SUBSTRATE PROCESSING METHOD AND SUBSTRATE PROCESSING SYSTEM

The substrate processing method addresses shape abnormalities in high aspect ratio semiconductor patterns by alternating temperature adjustments and reactive species application to form a protective film, enhancing precision and consistency in pattern formation.

JP7565763B2Active Publication Date: 2024-10-11TOKYO ELECTRON LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020190713
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-17
Publication Date
2024-10-11
Estimated Expiration
2040-11-17

AI Technical Summary

Technical Problem

The increasing aspect ratio of patterns in semiconductor manufacturing leads to shape abnormalities, such as bowing, during the etching process, which affects the precision and integrity of semiconductor devices.

Method used

A substrate processing method involving alternating temperature adjustments and reactive species application in multiple chambers to form a protective film on the sidewalls of recesses, followed by controlled etching to maintain a high aspect ratio while minimizing shape irregularities.

Benefits of technology

The method effectively suppresses shape abnormalities in semiconductor patterns, ensuring precise and consistent formation of high aspect ratio features by controlling the thickness and distribution of the protective film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565763000001
    Figure 0007565763000001
  • Figure 0007565763000002
    Figure 0007565763000002
  • Figure 0007565763000003
    Figure 0007565763000003
Patent Text Reader

Abstract

To suppress the abnormal shape of a semiconductor pattern.SOLUTION: A substrate processing method includes: a step a) of conveying a substrate including a first film with a concave part formed thereon and a mask into a first chamber; a step b) of setting a temperature of the substrate to 200°C or more; a step c-1) of sucking silicon-containing reaction species on a side wall of the concave part by supplying the silicon-containing reaction species into the first chamber; a step c-2) of forming a second film that is a silicon nitride film on the side wall of the concave part by supplying nitrogen-containing reaction species into the first chamber; a step d) of conveying the substrate into a second chamber; a step e) of setting a temperature of the substrate to 100°C or less; and a step f) of etching a bottom part of the concave part. The second film has a thickness of 20 nm or less, and a thickness ratio of the bottom part of the concave part to an upper side wall of the concave part is 0.7 or more. The steps a) to f) are executed repeatedly in this order until a ratio of a depth from an opening part of the mask to the bottom part of the concave part with respect to an opening size of the mask becomes 50 or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Various aspects and embodiments of the present disclosure relate to substrate processing methods and systems. [Background technology]

[0002] As semiconductor device integration progresses not only horizontally but also vertically, the aspect ratio of the patterns formed during the semiconductor device manufacturing process is also increasing. For example, in the manufacture of 3D NAND, channel holes are formed in a direction that penetrates multiple metal wiring layers. When forming 64-layer memory cells, the aspect ratio of the channel hole is as high as 45.

[0003] Various methods have been proposed to form high aspect ratio patterns with high accuracy. For example, a method has been proposed in which etching and film deposition are repeatedly performed in an opening formed in a dielectric material of a substrate to suppress lateral etching (Patent Document 1). Also, a method has been proposed in which etching and film deposition are combined to form a protective film to prevent lateral etching of a dielectric layer (Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] US Patent Application Publication No. 2016 / 0343580 [Patent Document 2] US Patent Application Publication No. 2018 / 0174858 Summary of the Invention [Problem to be solved by the invention]

[0005] The present disclosure provides a technique capable of suppressing shape abnormalities in semiconductor patterns. [Means for solving the problem]

[0006] One aspect of the present disclosure is a substrate processing method, including steps a), b), c), d), e), and f). In step a), a substrate having a first film to be processed, the first film having a recess formed therein, and a mask provided on the first film and having an opening formed at a position corresponding to the recess, is carried into a first chamber. In step b), the temperature of the substrate is adjusted to 200° C. or higher. In step c), a second film, which is a silicon nitride film, is formed on the sidewall of the recess. In step d), the substrate is carried into a second chamber different from the first chamber. In step e), the temperature of the substrate is adjusted to 100° C. or lower. In step f), the bottom of the recess is etched. In addition, step c) includes steps c-1) and c-2). In step c-1), silicon-containing reactive species are supplied into the first chamber, so that the silicon-containing reactive species are adsorbed on the sidewall of the recess. In step c-2), a nitrogen-containing reactive species is supplied into the first chamber, and the silicon-containing reactive species adsorbed on the sidewall of the recess is reacted with the nitrogen-containing reactive species to form a second film on the sidewall of the recess. The second film has a thickness of 20 nm or less, and a ratio of the film thickness at the bottom of the recess to the film thickness at the upper sidewall of the recess is 0.7 or more. Steps a) to f) are repeated in this order two or more times until a first aspect ratio, which is the ratio of the depth dimension from the opening of the mask to the bottom of the recess to the opening dimension of the mask, becomes 50 or more. Effect of the Invention

[0007] According to various aspects and embodiments of the present disclosure, shape abnormalities in a semiconductor pattern can be suppressed. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a flowchart showing an example of a substrate processing method according to the first embodiment of the present disclosure. [Diagram 2] FIG. 2 is a diagram showing an example of a process in the substrate processing method according to the first embodiment. [Diagram 3] FIG. 3 is a diagram showing an example of a distribution of a critical dimension (CD) in the depth direction of a recess. [Figure 4] FIG. 4 is a schematic plan view illustrating an example of a substrate processing system. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing an example of an etching apparatus. [Figure 6] FIG. 6 is a schematic cross-sectional view showing an example of a film forming apparatus. [Figure 7] FIG. 7 is a diagram showing an example of a process in the substrate processing method according to the second embodiment. [Figure 8] FIG. 8 is a diagram showing another example of the process in the substrate processing method according to the second embodiment. [Figure 9] FIG. 9 is a flowchart showing an example of a substrate processing method according to the modified example of the second embodiment. [Figure 10] FIG. 10 is a diagram showing an example of a process in a substrate processing method according to a modified example of the second embodiment. [Figure 11] FIG. 11 is a diagram showing another example of processing steps in the substrate processing method according to the modified example of the second embodiment. [Figure 12] FIG. 12 is a flowchart showing an example of a substrate processing method according to the third embodiment. [Figure 13] FIG. 13 is a diagram showing an example of a process in the substrate processing method according to the third embodiment. [Figure 14] FIG. 14 is a diagram showing an example of CD distribution in the depth direction of a recess. [Figure 15] FIG. 15 is a diagram showing an example of a cross section of a recess after processing. [Figure 16] FIG. 16 is a flowchart showing an example of a substrate processing method according to the fourth embodiment. [Figure 17] FIG. 17 is a diagram showing an example of a process in the substrate processing method according to the fourth embodiment. [Figure 18] FIG. 18 is a flowchart showing an example of a substrate processing method according to the fifth embodiment. [Figure 19] FIG. 19 is a diagram showing an example of a process in the substrate processing method according to the fifth embodiment. [Figure 20] FIG. 20 is a flowchart showing an example of a substrate processing method according to the sixth embodiment. [Figure 21] FIG. 21 is a diagram showing an example of an ESC zone. [Figure 22] FIG. 22 is a diagram showing another example of the zone of the ESC. [Diagram 23] FIG. 23 is a diagram showing another example of the zone of the ESC. [Figure 24] FIG. 24 is a diagram showing an example of a CD distribution in the depth direction of a recess under a first temperature condition. [Diagram 25] FIG. 25 is a diagram showing an example of a CD distribution in the depth direction of a recess under a second temperature condition. [Figure 26] FIG. 26 is a diagram summarizing the results of FIGS. [Figure 27] FIG. 27 is a diagram showing an example of a process in the substrate processing method according to the seventh embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, embodiments of the disclosed substrate processing method and substrate processing system will be described in detail with reference to the drawings. Note that the disclosed substrate processing method and substrate processing system are not limited to the following embodiments. In addition, each embodiment can be appropriately combined as long as the processing contents are not contradictory.

[0010] Incidentally, it is known that shape abnormalities occur when etching a pattern with a high aspect ratio. For example, when forming an opening in the vertical direction, a shape abnormality may occur in which the inner peripheral surface bulges in the horizontal direction. This type of shape abnormality is called bowing. A method of forming a protective film on the side wall of the opening has been proposed to suppress the occurrence of shape abnormalities. In forming fine patterns, it is further desirable to prevent the opening from being blocked by the protective film, and a decrease in the etching rate due to the formation of a film on the bottom of the opening.

[0011] In the following description, the term "pattern" refers to a shape formed on a substrate in general. The pattern refers to the entirety of a plurality of shapes formed on a substrate, such as holes, trenches, and lines and spaces. The term "recess" refers to a portion of a pattern formed on a substrate that is recessed in the thickness direction of the substrate. The recess has a "sidewall" that is the inner peripheral surface of the recess, a "bottom" that is the bottom of the recess, and a "top" that is the substrate surface adjacent to the sidewall and continues from the sidewall. The space surrounded by the top is called an "opening". The term "opening" is also used to refer to the entire space surrounded by the bottom and sidewall of the recess or any position in the space. The recess is an example of a semiconductor pattern.

[0012] (First embodiment) [Substrate processing method] Fig. 1 is a flowchart showing an example of a substrate processing method according to a first embodiment of the present disclosure. The process illustrated in Fig. 1 is executed by, for example, a substrate processing system 1 described later in Fig. 4. The process illustrated in Fig. 1 will be described below with reference to Fig. 2.

[0013] First, a substrate W to be processed is carried into an etching apparatus 12 (S10) to be described later. In step S10, the substrate W having a mask MA having a predetermined pattern formed thereon is carried into the etching apparatus 12, as shown in FIG. 2(A), for example. The mask MA has a thickness of 2000 nm or more, and an aspect ratio of 20 or more. The film EL is an example of a first film. The etching apparatus 12 is an example of a second chamber. In this embodiment, the film EL is a multilayer film having a silicon oxide film and a silicon nitride film. The film EL may be a silicon-containing film or an organic film. Examples of the silicon-containing film include a silicon nitride film, a polycrystalline silicon film, a carbon-containing silicon film, and a silicon germanium film. The silicon-containing film may be a laminated film including at least two of a polycrystalline silicon film, a silicon oxide film, and a silicon nitride film.

[0014] Next, the temperature of the substrate W is adjusted to a predetermined temperature not higher than 100° C. (S11). In step S11, the temperature of the substrate W is adjusted to, for example, 0° C.

[0015] Next, the film EL is etched in the thickness direction of the film EL along the shape of the mask MA (S12), thereby forming recesses, for example as shown in FIG. 2(B), in the film EL along the openings of the mask MA. The ratio of the depth dimension from the top of the mask MA to the bottom of the recess to the opening dimension of the mask MA is 10 or more.

[0016] Next, the control device of the substrate processing system 1 determines whether the process of step S12 has been performed for a predetermined time (S13). If the process of step S12 has not been performed for the predetermined time (S13: No), the process shown in step S12 is performed again. If the execution time of step S12 is long, not only does the depth of the recess increase, but shape abnormalities such as bowing occur on the sidewall of the recess. The predetermined time in step S13 is a time range in which shape abnormalities such as bowing do not occur on the sidewall of the recess formed in the film EL.

[0017] On the other hand, if the process of step S12 has been performed for a predetermined time (S13: Yes), the substrate W is unloaded from the etching apparatus 12. Then, the substrate W is loaded into a film forming apparatus 14 (S14), which will be described later. The film forming apparatus 14 is an example of a first chamber. Also, step S14 is an example of process a) and process h).

[0018] Next, the temperature of the substrate W is adjusted to a predetermined temperature of 200° C. or higher (S15). In step S15, the temperature of the substrate W is adjusted to, for example, 300° C. Step S15 is an example of step b) and step i).

[0019] Next, a protective film is formed on the surface of the recess (S16). In this embodiment, the protective film is, for example, a silicon nitride film. The protective film is an example of the second film. Step S16 is also an example of step c) and step j).

[0020] In step S16, first, a silicon-containing reactive species (precursor) gas is supplied to the surface of the substrate W (S160). Step S160 is an example of process c-1). As a result, precursor molecules are adsorbed on the surface of the substrate W. As the precursor gas, an aminosilane-based gas, for example, SiCl 4, Gases such as dichlorosilane (DCS) or hexachlorodisilane (HCDS) are used.

[0021] Before the start of step S160, a process for terminating the surface of the substrate W with an amino group may be performed by generating plasma from a gas containing nitrogen and hydrogen in the film forming apparatus 14. This allows the precursor molecules to be more efficiently adsorbed onto the surface of the substrate W. The process for terminating the surface of the substrate W with an amino group is an example of step c-0).

[0022] Next, the surface of the substrate W is purged with a purge gas (S161), thereby removing precursor molecules excessively adsorbed on the surface of the substrate W. As the purge gas, for example, a rare gas such as argon gas or an inert gas such as nitrogen gas is used.

[0023] Next, a nitrogen-containing reactive gas (reactive gas) is supplied to the surface of the substrate W (S162). Step S162 is an example of step c-2). As a result, the precursor molecules adsorbed on the surface of the substrate W are nitrided, and a protective film is formed on the surface of the substrate W. As the reactive gas, N2, NH3, or other gases are used. The nitrogen-containing reactive gas may be generated by plasmatizing the reactive gas. This allows the generation of more reactive nitrogen-containing reactive species, and the time required for forming the protective film can be shortened. In addition, when the pattern is a hole, it is difficult for the reactive gas molecules to reach the bottom of the pattern. In such a case, in step c-2), a bias voltage may be applied to the lower electrode on which the substrate W is placed. This allows the reactive gas molecules to reach the bottom of the pattern.

[0024] Next, the surface of the substrate W is purged with a purge gas (S163), thereby discharging the excess reactive gas.

[0025] Next, the control device of the substrate processing system 1 determines whether the process of step S16 has been performed for a predetermined time (S17). If the process of step S16 has not been performed for the predetermined time (S17: No), the process shown in step S16 is performed again. The predetermined time in step S17 is the time for the protective film formed on the side wall of the recess to reach a predetermined thickness. In this embodiment, the predetermined thickness is, for example, 20 nm or less. Preferably, the predetermined thickness may be, for example, 10 nm or less. Furthermore, preferably, the predetermined thickness may be, for example, 5 nm or less. This can reduce the time required to form the protective film. In addition, it is preferable that the ratio of the thickness of the protective film formed on the bottom side of the recess to the thickness of the protective film formed on the upper side of the recess is 0.7 or less.

[0026] On the other hand, if the process of step S16 has been performed for a predetermined time (S17: Yes), the substrate W is unloaded from the film forming apparatus 14. As a result, a protective film PF is formed on the surface of the recess of the film EL, for example, as shown in FIG. 2(C). Then, the substrate W is loaded again into the etching apparatus 12 (S18). Step S18 is an example of process d).

[0027] Here, in this embodiment, the film EL is a multilayer film of a silicon oxide film and a silicon nitride film, and molecules of silicon-containing reactive species are more likely to be adsorbed on the mask MA than on the film EL. Therefore, the protective film PF is formed thicker on the surface of the mask MA than on the surface of the film EL, as shown in FIG. 2(c), for example. Note that, in this embodiment, the film EL is formed by, for example, CVD (Chemical Vapor Deposition), and the protective film PF is formed by ALD (Atomic Layer Deposition). Therefore, the silicon nitride film included in the film EL and the protective film PF, which is a silicon nitride film, differ in at least one of the content ratio of silicon atoms and nitrogen atoms, the film density, and the crystal structure.

[0028] Next, the temperature of the substrate W is adjusted to a predetermined temperature not higher than 100° C. (S19). In step S19, the temperature of the substrate W is adjusted to, for example, 0° C. Step S19 is an example of step e).

[0029] Next, the bottom of the recess formed in the film EL is further etched along the shape of the mask MA (S20). Step S20 is an example of steps f) and k). Then, the control device determines whether the process of step S20 has been performed for a predetermined time (S21). If the process of step S20 has not been performed for the predetermined time (S21: No), the process shown in step S20 is performed again. If the execution time of step S20 is long, not only the depth of the recess increases, but also shape abnormalities occur in the sidewall of the recess. The predetermined time in step S20 is a time range in which shape abnormalities such as bowing do not occur in the sidewall of the recess formed in the film EL.

[0030] On the other hand, if the process of step S20 has been performed for a predetermined time (S21: Yes), the substrate W is unloaded from the etching device 12 (S22). As a result, a recess, for example as shown in FIG. 2(D), is formed in the film EL along the opening of the mask MA. Then, the substrate processing method shown in this flowchart ends.

[0031] Note that steps S14 to S21 may be repeated two or more times in this order. This allows recesses with a high aspect ratio (A / R) to be formed in the film EL while suppressing shape abnormalities in the recesses. Furthermore, when steps S14 to S21 are repeatedly performed, at least one of the time for which the silicon-containing reactive species is supplied and the time for which the nitrogen-containing reactive species is supplied may be controlled to be longer in the later performed steps S14 to S21 than in the earlier performed steps S14 to S21.

[0032] [Recess CD] Fig. 3 is a diagram showing an example of CD distribution in the depth direction of the recesses. The depth of the recesses is defined as a negative depth on the film EL side and a positive depth on the mask MA side, with the boundary between the mask MA and the film EL as a reference, as shown in Fig. 3(A), for example.

[0033] The comparative example in Figure 3(B) shows the distribution of CD in the depth direction of the recess when the recess is etched without forming a protective film PF. In the comparative example, the CD is large near the boundary between the mask MA and the film EL. Also, as the depth of the recess increases in the negative direction, the CD decreases. If a rectangular cross-sectional shape is the ideal shape of a recess, the cross-sectional shape of the recess in the comparative example is abnormal to the ideal shape of the recess.

[0034] On the other hand, in the recesses formed by the method of this embodiment, as shown in Fig. 3(B), the increase in CD near the boundary between the mask MA and the film EL is suppressed to be smaller than that in the comparative example. Also in this embodiment, the CD decreases as the depth of the recess increases in the negative direction, but the amount of decrease is suppressed to be smaller than that in the comparative example. That is, the method of this embodiment suppresses shape abnormalities in the recesses.

[0035] [Configuration of substrate processing system 1] The process illustrated in Fig. 1 is performed, for example, by a substrate processing system 1 shown in Fig. 4. Fig. 4 is a schematic plan view showing an example of the substrate processing system 1. For convenience of explanation, the upper parts of some of the devices are drawn transparently in Fig. 4. The substrate processing system 1 in this embodiment is a multi-chamber type vacuum processing system. The substrate processing system 1 uses a plurality of etching devices 12 and film forming devices 14 to form recesses of a predetermined pattern on a substrate W to be processed.

[0036] The substrate processing system 1 includes a main body 10 and a control device 100 that controls each part of the main body 10. The main body 10 includes a vacuum transfer chamber 11. The vacuum transfer chamber 11 has a hexagonal shape in plan view, and a plurality of etching devices 12 are connected to two side walls of the vacuum transfer chamber 11 via gate valves G1. A vacuum transfer chamber 13 is connected to the other side wall of the vacuum transfer chamber 11 via gate valves G2. A storage chamber 15 is connected to the other side wall of the vacuum transfer chamber 11 via gate valves G4. A load lock chamber 16 is connected to the other two side walls of the vacuum transfer chamber 11 via gate valves G5.

[0037] The inside of the vacuum transfer chamber 11 is evacuated by a vacuum pump and maintained at a predetermined vacuum level. A transfer device 110 such as a robot arm is provided inside the vacuum transfer chamber 11. The transfer device 110 moves inside the vacuum transfer chamber 11 along a guide rail 111 provided inside the vacuum transfer chamber 11. The transfer device 110 transfers the substrate W between the etching device 12, the vacuum transfer chamber 13, the storage chamber 15, and the load lock chamber 16. The transfer device 110 is an example of a second transfer device.

[0038] Each of the etching devices 12 is a single-wafer etching device, and etches a film EL below the mask MA along the shape of the mask MA provided on the substrate W. The vacuum transfer chamber 13 is connected to the film forming device 14 via a gate valve G3. A transfer device 13a such as a robot arm for transferring the substrate W is provided in the vacuum transfer chamber 13. The transfer device 13a transfers the substrate W between the vacuum transfer chamber 11 and the film forming device 14. The transfer device 13a receives the substrate W from the transfer device 110 in the vacuum transfer chamber 11 or the vacuum transfer chamber 13, and places the substrate W in a predetermined boat 144 provided in the film forming device 14. The transfer device 13a is an example of a first transfer device.

[0039] The film forming apparatus 14 forms a protective film PF in the recesses of the substrate W. In this embodiment, the film forming apparatus 14 is a batch-type film forming apparatus capable of forming the protective film PF on multiple substrates W at once. In the film forming apparatus 14, multiple substrates W are accommodated lined up, for example, in the vertical direction. This makes it possible to reduce the footprint of the film forming apparatus 14. Note that, in the film forming apparatus 14, multiple substrates W may be accommodated lined up in a direction other than the vertical direction. The transport device 13a can move the substrate W in the vertical direction. By repeating the etching of the film EL by the etching device 12 and the formation of the protective film PF by the film forming apparatus 14, recesses with a high A / R and reduced shape abnormality in the film EL are formed in the substrate W.

[0040] The substrate W etched by the etching apparatus 12 is temporarily stored in the storage chamber 15 until it is carried into the film forming apparatus 14. In addition, the substrate W on which the protective film PF is formed by the film forming apparatus 14 is temporarily stored in the storage chamber 15 until it is carried into the etching apparatus 12.

[0041] Each load lock chamber 16 is connected to an atmospheric transfer chamber 17 via a gate valve G6. A plurality of ports 18 are provided on the side of the atmospheric transfer chamber 17 for attaching a carrier C such as a FOUP (Front-Opening Unified Pod) that accommodates a substrate W. An alignment chamber 17c for aligning the substrate W is also provided on the side wall of the atmospheric transfer chamber 17. A downflow of clean air is also formed within the atmospheric transfer chamber 17.

[0042] A transfer device 17a such as a robot arm is provided in the atmospheric transfer chamber 17. The transfer device 17a moves within the atmospheric transfer chamber 17 along guide rails 17b provided in the atmospheric transfer chamber 17. The transfer device 17a transfers the substrate W between each carrier C, each load lock chamber 16, and the alignment chamber 17c.

[0043] The control device 100 has a memory, a processor, and an input / output interface. The memory stores a program executed by the processor, a recipe including the conditions for each process, and the like. The processor executes the program read from the memory, and controls each part of the main body 10 via the input / output interface based on the recipe stored in the memory.

[0044] [Configuration of the etching device 12] 5 is a schematic cross-sectional view showing an example of the etching apparatus 12. In this embodiment, the etching apparatus 12 is a single-wafer type plasma etching apparatus equipped with parallel plate electrodes. The etching apparatus 12 has a processing vessel 120 having a substantially cylindrical shape. The processing vessel 120 has a processing space S p The processing vessel 120 is made of, for example, aluminum, and its inner wall surface is anodized. The processing vessel 120 is safety grounded.

[0045] A substantially cylindrical support member 121 is provided on the bottom of the processing vessel 120. The support member 121 is made of an insulating material that can contain oxygen, such as quartz. The support member 121 extends, for example, vertically from the bottom of the processing vessel 120 within the processing vessel 120. A mounting table PD is provided within the processing vessel 120. The mounting table PD is supported by the support member 121.

[0046] The mounting table PD holds the substrate W on the upper surface of the mounting table PD. The surface FW of the substrate W to be etched by the etching device 12 is the surface opposite to the back surface of the substrate W that contacts the upper surface of the mounting table PD, and faces the upper electrode 130. The mounting table PD has a lower electrode LE and an electrostatic chuck ESC. The lower electrode LE includes a first plate 118a and a second plate 118b that are substantially disk-shaped. The first plate 118a and the second plate 118b are made of a metal such as aluminum. The second plate 118b is provided on the first plate 118a and is electrically connected to the first plate 118a.

[0047] An electrostatic chuck ESC is provided on the second plate 118b. The electrostatic chuck ESC has a structure in which an electrode, which is a conductive film, is disposed between a pair of insulating layers or between a pair of insulating sheets. A DC power supply 122 is electrically connected to the electrode of the electrostatic chuck ESC via a switch 123. When the substrate W is placed on the mounting table PD, the back surface (the surface opposite to the surface FW) of the substrate W contacts the electrostatic chuck ESC. The electrostatic chuck ESC attracts the substrate W by electrostatic force such as Coulomb force generated by a DC voltage from the DC power supply 122. This allows the electrostatic chuck ESC to hold the substrate W.

[0048] An edge ring ER is disposed on the periphery of the second plate 118b so as to surround the edge of the substrate W and the electrostatic chuck ESC. The edge ring ER is provided to improve the uniformity of etching. The edge ring ER is made of a material appropriately selected depending on the material of the film to be etched, and may be made of, for example, silicon or quartz.

[0049] A flow path 124 is provided inside the second plate 118b. A coolant is supplied to the flow path 124 from a chiller unit (not shown) provided outside the processing vessel 120 via a pipe 126a. The coolant supplied to the flow path 124 via the pipe 126a is returned to the chiller unit via the pipe 126b. Thus, the coolant whose temperature is controlled by the chiller unit circulates inside the flow path 124. By controlling the temperature of the coolant, the temperature of the substrate W can be controlled via the electrostatic chuck ESC.

[0050] The mounting table PD is provided with a pipe 128. The pipe 128 supplies a heat transfer gas from a heat transfer gas supply mechanism (not shown) to between the electrostatic chuck ESC and the substrate W. The heat transfer gas may be, for example, helium gas.

[0051] The mounting table PD is provided with a heater HT for adjusting the temperature of the substrate W. The heater HT is built in the electrostatic chuck ESC. A heater power source HP is connected to the heater HT. When power is supplied from the heater power source HP to the heater HT, the temperature of the electrostatic chuck ESC is adjusted, and the temperature of the substrate W placed on the electrostatic chuck ESC is adjusted. The heater HT may be embedded in the second plate 118b. When etching the substrate W, the heater HT adjusts the temperature of the substrate W to 100° C. or less, such as 0° C., by controlling the amount of heating relative to the amount of cooling by the coolant flowing through the flow path 124. The heater HT is an example of a second temperature adjustment unit.

[0052] An upper electrode 130 is provided above the mounting table PD. The upper electrode 130 is disposed above the mounting table PD so as to face the mounting table PD. The lower electrode LE and the upper electrode 130 are disposed substantially parallel to each other and form parallel plate electrodes. A processing space S for processing the substrate W is defined between the upper electrode 130 and the lower electrode LE. p is provided.

[0053] The upper electrode 130 is supported on the upper part of the processing vessel 120 via an insulating member 132. The insulating member 132 is made of an insulating material that can contain oxygen, such as quartz. The upper electrode 130 includes an electrode plate 134 and an electrode support 136. The electrode plate 134 is disposed in the processing space S. p 1, and a plurality of gas discharge ports 134a are formed in the electrode plate 134. The electrode plate 134 contains, for example, silicon. The electrode plate 134 may be, for example, silicon.

[0054] The electrode support 136 is made of a conductive material such as aluminum, and detachably supports the electrode plate 134. The electrode support 136 may have a water-cooled structure. A gas diffusion chamber 136a is provided inside the electrode support 136. The gas diffusion chamber 136a allows gas to flow through a plurality of gas circulation ports 136b that communicate with the gas discharge port 134a into the processing space S. p The gas diffusion chamber 136a is connected to a pipe 138 via a gas inlet 136c. The pipe 138 is connected to a gas supply unit 150.

[0055] The main body 10 has a first RF (Radio Frequency) power supply 162 and a second RF power supply 164. The first RF power supply 162 is a power supply that generates a first RF power for generating plasma, and generates an RF power with a frequency of 27 to 100 MHz, for example, 60 MHz. The first RF power supply 162 outputs the generated RF power in a pulsed form. The frequency of the pulse can be controlled, for example, in the range of 0.1 to 50 kHz, and the duty ratio of the pulse can be controlled, for example, in the range of 5 to 100%. The first RF power supply 162 is connected to the lower electrode LE via a matching device 166. The matching device 166 is a circuit for matching the output impedance of the first RF power supply 162 with the input impedance on the load side (lower electrode LE side). The first RF power supply 162 may be connected to the upper electrode 130 via the matching device 166.

[0056] The second RF power supply 164 is a power supply that generates a second RF wave power for attracting ions into the substrate W, i.e., an RF bias power, and generates an RF bias power having a frequency within a range of 400 kHz to 40.68 MHz, for example, a frequency of 13.56 MHz. The second RF power supply 164 also outputs the generated RF bias power in a pulsed form. The frequency of the pulse can be controlled within a range of, for example, 0.1 to 50 kHz, and the duty ratio of the pulse can be controlled within a range of, for example, 5 to 100%. The second RF power supply 164 is connected to the substrate processing system 1LE via a matching device 168. The matching device 168 is a circuit for matching the output impedance of the second RF power supply 164 with the input impedance on the load side (lower electrode LE side).

[0057] A power supply 160 is connected to the electrode support 136 of the upper electrode 130. The power supply 160 supplies power to the processing space S p A voltage is applied to the upper electrode 130 to attract the positive ions present in the processing space S to the electrode plate 134. The power supply 160 is, for example, a DC power supply that generates a negative DC voltage. When such a voltage is applied from the power supply 160 to the upper electrode 130, p Positive ions present in the electrode plate 134 collide with the electrode plate 134. This can cause secondary electrons, silicon, or both to be emitted from the electrode plate 134.

[0058] An exhaust plate 155 made of, for example, an aluminum material coated with ceramics such as Y2O3 is provided on the bottom side of the processing vessel 120 and between the support member 121 and the sidewall of the processing vessel 120. An exhaust port 120e is formed below the exhaust plate 155 and at the bottom of the processing vessel 120. An exhaust device 158 is connected to the exhaust port 120e via an exhaust pipe 157. The exhaust device 158 has a vacuum pump such as a turbo molecular pump and can reduce the pressure in the space inside the processing vessel 120 to a predetermined vacuum level.

[0059] An opening 120g for loading and unloading the substrate W is formed in a sidewall of the processing vessel 120. The opening 120g is opened and closed by a gate valve G1. A gas inlet 157a is provided in the sidewall of the processing vessel 120. The gas inlet 157a is provided on the side of the substrate W placed on the mounting table PD in the processing vessel 120. A gas supply unit 150 is connected to the gas inlet 157a via a pipe 139. The gas supply unit 150 is an example of a second gas supply unit.

[0060] The gas supply unit 150 includes a gas source group 151, a flow rate controller group 152, and a valve group 153. The gas source group 151 includes a plurality of gas sources. The plurality of gas sources include a fluorocarbon gas (C x F y The gas source may include various gas sources such as a gas source (x and y are integers from 1 to 10) and an inert gas source. As the inert gas, any gas such as nitrogen gas, argon gas, or helium gas may be used.

[0061] The flow rate controller group 152 includes a plurality of flow rate controllers such as mass flow controllers, and the valve group 153 includes a plurality of valves. Each of the plurality of gas sources included in the gas source group 151 is connected to the pipe 138 and the pipe 139 via a corresponding flow rate controller included in the flow rate controller group 152 and a corresponding valve included in the valve group 153. Thus, the main body 10 supplies gas supplied from one or more selected gas sources among the plurality of gas sources of the gas source group 151 at individually adjusted flow rates to the processing space S in the processing vessel 120 via the pipe 138 and the pipe 139. p can be supplied to.

[0062] A deposit shield 154 is detachably provided on the inner wall of the processing vessel 120. The deposit shield 154 is also provided on the outer periphery of the support member 121. The deposit shield 154 prevents etching by-products (deposits) from adhering to members inside the processing vessel 120. The deposit shield 154 may be formed by coating a member made of aluminum or the like with ceramics such as Y2O3. In addition to Y2O3, the deposit shield 154 may be formed of a material containing oxygen, such as quartz.

[0063] [Configuration of the film forming apparatus 14] 6 is a schematic cross-sectional view showing an example of the film forming apparatus 14. In FIG. 6, the vacuum transfer chamber 13 is also shown.

[0064] A transfer device 13a is provided in the vacuum transfer chamber 13. The transfer device 13a can move the substrate W in a direction intersecting a horizontal plane (for example, a vertical direction).

[0065] The film forming apparatus 14 has a generally cylindrical outer wall 140 with a ceiling, and an inner wall 141 provided inside the outer wall 140. The outer wall 140 and the inner wall 141 are formed of, for example, quartz. An annular space 143 is formed between the outer wall 140 and the inner wall 141. The outer wall 140 and the inner wall 141 are joined to a base member 145.

[0066] A boat 144 is provided in the processing chamber 142 inside the inner wall 141. The boat 144 holds a plurality of substrates W arranged in a direction intersecting a horizontal plane (for example, a vertical direction). This allows the film forming apparatus 14 to collectively form a protective film PF on the plurality of substrates W. Furthermore, by holding a plurality of substrates W arranged in a direction intersecting a horizontal plane (for example, a vertical direction), the footprint of the film forming apparatus 14 can be reduced.

[0067] Gas is supplied through a pipe 148a into the processing chamber 142 inside the inner wall 141. The gas supplied into the processing chamber 142 passes through annular space 143 between the outer wall 140 and the inner wall 141, and is exhausted from a pipe 148b.

[0068] A gas supply unit 146 is connected to the pipe 148a. The gas supply unit 146 is an example of a first gas supply unit. The gas supply unit 146 has a plurality of valves 1460a to 1460c, a plurality of MFCs (Mass Flow Controllers) 1461a to 1461c, and a plurality of gas sources 1462a to 1462c. The gas source 1462a is a supply source of a precursor gas. The gas source 1462b is a supply source of a purge gas. The gas source 1462c is a supply source of a reactive gas. In this embodiment, the precursor gas is a gas containing a silicon-containing reactive species, such as SiCl4, dichlorosilane (DCS), or hexachlorodisilane (HCDS). In this embodiment, the purge gas is, for example, a rare gas such as argon gas, or an inert gas such as nitrogen gas. In this embodiment, the reactive gas is a gas that includes a nitrogen-containing reactive species, such as N2 or NH3.

[0069] A heater 147 is provided on the inner wall 141. The heater 147 adjusts the temperature of the substrate W to, for example, 200° C. or higher during the formation of the protective film PF. In this embodiment, the heater 147 adjusts the temperature of the substrate W to, for example, 300° C. during the formation of the protective film PF. The heater 147 is an example of a first temperature adjustment unit.

[0070] The first embodiment has been described above. As described above, the substrate processing method in this embodiment includes steps a), b), c), d), e), and f). In step a), a substrate W having a recess formed in a film EL to be processed is carried into a film forming apparatus 14. In step b), the temperature of the substrate W is adjusted to 200° C. or higher, and in step c), a protective film PF, which is a silicon nitride film, is formed on the side wall of the recess. In step d), the substrate W is carried into an etching apparatus 12 different from the film forming apparatus 14. In step e), the temperature of the substrate W is adjusted to 100° C. or lower. In step f), the bottom of the recess is etched. This makes it possible to suppress shape abnormalities of a semiconductor pattern formed on the substrate W.

[0071] In the above embodiment, step c) includes steps c-1) and c-2). In step c-1), silicon-containing reactive species are supplied into the film forming apparatus 14, and the silicon-containing reactive species are adsorbed on the sidewall of the recess. In step c-2), nitrogen-containing reactive species are supplied into the film forming apparatus 14, and the silicon-containing reactive species adsorbed on the sidewall of the recess reacts with the nitrogen-containing reactive species, forming a protective film PF on the sidewall of the recess. This allows a protective film PF of a predetermined thickness to be formed on the sidewall of the recess.

[0072] In the above embodiment, the nitrogen-containing reactive species may be generated by converting a nitrogen-containing gas into plasma, which can generate more reactive nitrogen-containing reactive species and shorten the time required to form the protective film PF.

[0073] In the above embodiment, step c) may include step c-0) performed before step c-1). In step c-0), a gas containing nitrogen and hydrogen is turned into plasma in the film forming apparatus 14, so that the surface of the substrate W is terminated with amino groups. This allows the precursor molecules to be adsorbed on the surface of the substrate W more efficiently.

[0074] In the above embodiment, in step c), it is preferable that a protective film PF of 20 nm or less is formed on the side wall of the recess. More preferably, in step c), a protective film PF of 10 nm or less may be formed on the side wall of the recess. This can reduce the time required to form the protective film PF.

[0075] In the above embodiment, the substrate W is provided with a mask MA on the film EL, and in step c), the protective film PF is also formed on the surface of the mask MA. The thickness of the protective film PF formed on the surface of the mask MA is thicker than the thickness of the protective film PF formed on the side walls of the recesses. This makes it possible to reduce the amount of loss of the mask MA during etching.

[0076] In the above-described embodiment, the film EL has a silicon oxide film and a silicon nitride film, and the silicon nitride film included in the film EL and the protective film PF differ from each other in at least one of the content ratio of silicon atoms and nitrogen atoms, the film density, and the crystal structure.

[0077] In the above embodiment, steps a) to f) may be repeated two or more times in this order, thereby forming recesses with a high A / R ratio while suppressing shape abnormalities in the recesses.

[0078] The substrate processing method in the above-described embodiment is performed using a substrate processing system 1 including a batch-type film forming apparatus 14 capable of accommodating a plurality of substrates W, and a plurality of single-wafer etching apparatuses 12. This makes it possible to efficiently form recesses having a predetermined shape on the plurality of substrates W.

[0079] Further, the substrate processing system 1 in the above embodiment includes a film forming apparatus 14, a heater 147, a gas supply unit 146, an etching apparatus 12, a heater HT, a gas supply unit 150, a transport device, and a control device 100. The film forming apparatus 14 accommodates a substrate W having a recess formed in a film EL to be processed. The heater 147 adjusts the temperature of the substrate W accommodated in the film forming apparatus 14. The gas supply unit 146 supplies gas into the film forming apparatus 14. The etching apparatus 12 accommodates the substrate W and is different from the film forming apparatus 14. The heater HT adjusts the temperature of the substrate W accommodated in the etching apparatus 12. The gas supply unit 150 supplies gas into the etching apparatus 12. The transport device 110 and the transport device 13a transport the substrate W between the film forming apparatus 14 and the etching apparatus 12. The control device 100 executes steps a) to f). The control device 100 controls the transport device to transport the substrate W into the film forming device 14 in step a). The control device 100 also controls the heater 147 in step b) so that the temperature of the substrate W is 200° C. or higher. The control device 100 also controls the gas supply unit 146 in step c) so that a protective film PF, which is a silicon nitride film, is formed on the side wall of the recess. The control device 100 also controls the transport device to transport the substrate W into the etching device 12 in step d). The control device 100 also controls the heater HT in step e) so that the temperature of the substrate W is 100° C. or lower. The control device 100 also controls the gas supply unit 150 in step f) so that the bottom of the recess is etched. This makes it possible to suppress shape abnormalities of the semiconductor pattern formed on the substrate W.

[0080] In the above embodiment, the film forming apparatus 14 is, for example, a batch-type film forming apparatus capable of accommodating a plurality of substrates W in the vertical direction, and the etching apparatus 12 is a single-wafer etching apparatus. This makes it possible to reduce the footprint of the substrate processing system 1.

[0081] In the above embodiment, the transport device includes the transport device 110 and the transport device 13a. The transport device 13a transports the substrate W into the film forming device 14 and transports the substrate W out of the film forming device 14. The transport device 110 transports the substrate W into the etching device 12 and transports the substrate W out of the etching device 12. The transport device 13a is capable of transporting the substrate W in the vertical direction. This allows the footprint of the substrate processing system 1 to be reduced.

[0082] In the above embodiment, the substrate processing system 1 further includes a storage chamber 15 for storing the substrate W after step c) has been performed until step d) is started after step c) has been performed. This allows the substrate processing system 1 to efficiently process a plurality of substrates W.

[0083] Second embodiment In the first embodiment, the protective film PF is conformally formed on the sidewall of the recess formed in the film EL of the substrate W. In contrast, in the present embodiment, the processing conditions are set so that the self-limiting adsorption or reaction on the surface of the recess of the film EL is not completed. At least the following two processing modes can be given. (1) The precursor P is adsorbed onto the entire surface of the recesses of the film EL. After that, the reactant gas R is introduced and controlled so as not to reach the entire surface of the recesses. (2) The precursor P is adsorbed only to a part of the surface of the recessed portion of the film EL, and then the reactant gas is introduced to react only with the surface portion of the recessed portion to which the precursor P is adsorbed.

[0084] This allows a thicker protective film PF to be formed on the sidewall of the recess of the film EL in the portion where the recess extends in the width direction CD, and further suppresses shape abnormalities in the recess. In this embodiment, the protective film PF is formed on the sidewall of the recess by a method similar to the substrate processing method illustrated in Fig. 1, except for the points described below. Also in this embodiment, the substrate W is processed by the substrate processing system 1 described with reference to Figs. 4 to 6.

[0085] 7 is a diagram showing an example of a process in the substrate processing method of the second embodiment. In this embodiment, first, a precursor P is introduced into a film forming apparatus 14 in which a substrate W is placed (FIG. 7(A)). Molecules of the precursor P enter a recess through an opening OP formed in a film EL of the substrate W and are adsorbed onto the surface of the recess. By providing a processing time sufficient for the molecules of the precursor P to be adsorbed onto the entire surface of the recess, the molecules of the precursor P are adsorbed onto the entire surface of the recess (FIG. 7(B)). When the adsorption of the precursor P is completed, the surface of the substrate W is purged.

[0086] Next, the reactive gas R is introduced into the film forming apparatus 14 (FIG. 7C). The introduced reactive gas R penetrates into the recess while reacting with the precursor P adsorbed on the surface of the recess. As a result, a protective film PF is gradually formed from the top of the recess. Here, before the formation of the protective film PF reaches the bottom of the recess, the supply of the reactive gas R is stopped and the surface of the substrate W is purged. As a result, while using the ALD technique, the protective film PF can be formed only on the upper part of the side wall of the recess, rather than on the entire side wall of the recess (FIG. 7D). In FIG. 7D, the protective film PF is formed, for example, on the surface of the mask MA and near the boundary between the mask MA and the film EL on the side wall of the recess, but not on the lower part and bottom of the side wall of the recess.

[0087] 8 is a diagram showing another example of the process in the substrate processing method of the second embodiment. In the example of FIG. 8, the molecules of the precursor P are adsorbed only on the upper part of the film EL (FIG. 8(A)). Then, after the molecules of the precursor P are purged, the reaction gas R is introduced into the film forming apparatus 14 (FIG. 8(B)). At this time, the reaction gas R reacts with the molecules of the precursor P only at the positions where the molecules of the precursor P are adsorbed, so that the protective film PF is formed only on the upper part of the recess (FIG. 8(C)).

[0088] As described above, in the substrate processing method according to the present embodiment, the reaction between the precursor P and the reactive gas R occurs only at a predetermined portion of the sidewall of the recess. In this case, for example, a processing condition is set such that the adsorption of the precursor P molecules occurs at the upper portion of the sidewall of the recess, or a processing condition is set such that the reaction of the reactive gas R occurs only at the upper portion of the sidewall of the recess. Parameters for setting such processing conditions include, for example, the temperature of the substrate W, the pressure in the film forming apparatus 14, the flow rate and introduction time of the precursor P to be introduced, the flow rate and introduction time of the reactive gas R to be introduced, and the processing time. In addition, in the case of a process using plasma, the frequency and magnitude of the RF power supplied for plasma generation may be adjusted.

[0089] In the second embodiment described above, when a recess is formed in a shape in which the width of the recess decreases from the top to the bottom, the protective film PF can suppress the dimensional variation of the sidewall while realizing control to increase the dimension of the bottom. In addition, a modified example of the second embodiment that can further improve the degree of freedom in controlling the shape of the recess to be formed will be described below.

[0090] (Substrate Processing Method in Modification) Fig. 9 is a flow chart showing an example of a substrate processing method according to a modification of the second embodiment. Fig. 9 shows only the parts different from the substrate processing method according to the first embodiment shown in Fig. 1. In this modification, a measuring device for measuring the CD of the bottom of the recess is provided in the storage chamber 15 of the substrate processing system 1 shown in Fig. 4.

[0091] In this modification, first, the processes of steps S10 to S13 illustrated in Fig. 1 are executed. Then, the processes of steps S14 to S21 illustrated in Fig. 1 are executed. Then, the substrate W is carried out from the etching apparatus 12 and carried into the storage chamber 15. Then, the CD of the bottom of the recess is measured by a measuring device provided in the storage chamber 15 (S30). The method for measuring the CD of the bottom of the recess is not particularly limited, and may be measured by an optical method, for example.

[0092] Next, the control device 100 judges whether the measured CD of the bottom of the recess is equal to or greater than a predetermined value (S31). If the CD of the bottom of the recess is less than the predetermined value (S31: No), the process shown in step S14 is executed again. On the other hand, if the CD of the bottom of the recess is equal to or greater than the predetermined value (S31: Yes), the process shown in step S22 is executed.

[0093] Fig. 10 is a diagram showing an example of a process in the substrate processing method according to the modified example of the second embodiment. In the substrate processing method according to the modified example of the second embodiment, in step S10, as shown in Fig. 10(A), for example, a film EL is laminated on a base material BM, and a substrate W having a mask MA having a predetermined pattern formed thereon is loaded into an etching apparatus 12. Then, steps S11 to S13 are performed, and a recess is formed in the film EL according to the pattern formed on the mask MA, as shown in Fig. 10(B), for example. In the example of Fig. 10(B), the bottom of the recess reaches the base material BM.

[0094] Then, steps S14 to S17 are performed to deposit a protective film PF on the sidewalls of the recesses. At this time, the protective film PF is deposited under processing conditions such that the reaction between the precursor P and the reaction gas R occurs only on the upper part of the sidewalls of the recesses. As a result, the protective film PF is deposited only on the surface of the mask MA and the upper part of the sidewalls of the recesses, for example, as shown in Fig. 10(C). Then, the processing of S18 to S21 is performed.

[0095] Then, the CD of the bottom of the recess is measured, and the processes of steps S14 to S21 are repeated until the CD of the bottom of the recess becomes equal to or greater than a predetermined value. As a result, the cross-sectional shape of the recess becomes, for example, as shown in Fig. 10(D), and shape abnormalities in the recess are suppressed.

[0096] In the example of Fig. 10, the protective film PF is formed on the side wall of the recess after the bottom of the recess reaches the substrate BM by etching, but the disclosed technology is not limited to this. For example, as another example, as illustrated in (A) to (D) of Fig. 11, the protective film PF may be formed on the side wall of the recess before the bottom of the recess formed by etching reaches the substrate BM.

[0097] In the example of FIG. 11, the protective film PF is formed on a part of the side wall of the recess, but as another example, the protective film PF may be formed on the entire side wall and bottom of the recess.

[0098] (Third embodiment) In the second embodiment, at least one of the precursor P and the reaction gas R is supplied only to a predetermined portion of the side wall of the recess, so that the reaction between the precursor P and the reaction gas R occurs only in the predetermined portion of the side wall of the recess. In contrast, in the present embodiment, an inhibitor (hereinafter also referred to as an inhibitor) that inhibits the adsorption of the precursor P is formed in advance on a part of the surface of the recess, thereby controlling the adsorption position of the precursor P. This allows the precursor P to be adsorbed at a position in the recess other than the position where the inhibitor is formed, and a protective film PF can be formed at a position in the recess other than the position where the inhibitor is formed. In this embodiment, the protective film PF is formed on the side wall of the recess by a method similar to the substrate processing method exemplified in FIG. 1, except for the points described below. In this embodiment, the substrate W is also processed by the substrate processing system 1 described with reference to FIGS. 4 to 6.

[0099] (Substrate processing method) Fig. 12 is a flow chart showing an example of a substrate processing method in the third embodiment. In this embodiment, first, the processes of steps S10 to S14 illustrated in Fig. 1 are performed. Then, an inhibitor layer IN is formed as an inhibitor in a partial region of the surface of the recess (S40). Then, the processes of steps S15 to S22 illustrated in Fig. 1 are performed.

[0100] 13 is a diagram showing an example of a process in the substrate processing method of the third embodiment. In step S40, as shown in FIG. 13(A), a gas containing inhibitor I is supplied to the surface of the substrate W. The gas containing inhibitor I is, for example, a gas containing carbon. Examples of the gas containing carbon include fluorocarbon gas, fluorohydrocarbon gas, and hydrocarbon gas. The gas containing inhibitor I is, for example, plasmatized and supplied to the surface of the substrate W. As a result, an inhibitor layer IN is formed in the recess of the substrate W, as shown in FIG. 13(B).

[0101] When a fluorocarbon gas is used as the gas containing the inhibitor I, a fluorocarbon film is formed as the inhibitor layer IN in the recess. When a fluorohydrocarbon gas is used as the gas containing the inhibitor I, a fluorohydrocarbon film is formed as the inhibitor layer IN in the recess. When a hydrocarbon gas is used as the gas containing the inhibitor I, a hydrocarbon film is formed as the inhibitor layer IN in the recess. The fluorocarbon film, the fluorohydrocarbon film, and the hydrocarbon film are all hydrophobic films. By adjusting the processing conditions of the plasma CVD, the inhibitor layer IN can be formed in any region of the recess. In the example of FIG. 13(B), the inhibitor layer IN is formed on the top of the mask MA and on the bottom of the recess.

[0102] Next, in step S15, the temperature of the substrate W is adjusted to 200° C. or higher, and in step S160, a precursor P is supplied into the film forming apparatus 14, as shown in, for example, FIG. 13(C). At this time, the molecules of the precursor P are not adsorbed to the portion where the inhibitor layer IN is formed. Therefore, the molecules of the precursor P are selectively adsorbed to the side wall of the recess where the inhibitor layer IN is not formed, as shown in, for example, FIG. 13(D).

[0103] Then, in step S161, the surface of the substrate W is purged, and in step S162, a reactive gas R is supplied into the film forming apparatus 14. As a result, the molecules of the precursor P selectively adsorbed on the side walls of the recesses on which the inhibitor layer IN is not formed react with the reactive gas R, and a protective film PF is formed on the side walls of the recesses as shown in Fig. 13(D). At this time, by performing purging in step S163 before the molecules of the reactive gas R reach the bottom of the recesses, it is possible to form a protective film PF on the side walls of the recesses that is thicker at the top and thinner at the bottom, for example, as shown in Fig. 13(D).

[0104] In this way, when the protective film PF is formed using the inhibitor I, the formation position and film thickness of the protective film PF can be further adjusted. In addition, the formation position of the protective film PF can be controlled by the temperature of the substrate W, the pressure in the film forming apparatus 14, and the like. Therefore, according to this embodiment, the formation of the protective film PF on the upper part of the mask MA can be prevented by the inhibitor I, and the opening of the recess can also be prevented from being blocked when the protective film PF is formed.

[0105] [Recess CD] FIG. 14 is a diagram showing an example of CD distribution in the depth direction of the recess. FIG. 14 shows CD distribution in the depth direction of the recess based on the interface between the mask MA and the film EL in the recess in the initial state and in the recess after the protective film PF is formed. The amount of the protective film PF formed on the side wall (one side) of the recess is a value obtained by dividing the difference between the CD in the initial state and the CD after the protective film PF is formed by half. In FIG. 14(A), the dashed line shows the CD distribution in the initial state of the recess (initial state). Moreover, the dashed line shows the CD distribution when the protective film PF is formed on the recess in the initial state by using the substrate processing method in the first embodiment (Reference Example 1). Moreover, the solid line shows the CD distribution when the protective film PF is formed by normal ALD after the inhibitor layer IN is formed on the recess in the initial state by plasma CVD (Reference Example 2). Moreover, in FIG. 14(B), the dashed line shows the CD distribution in the initial state of the recess (initial state). The dashed and dotted lines show the CD distribution when a protective film PF is formed on the recesses in the initial state using the substrate processing method according to the second embodiment (second embodiment), and the solid lines show the CD distribution when a protective film PF is formed on the recesses in the initial state using the substrate processing method according to the third embodiment (third embodiment).

[0106] As shown in FIG. 14(A), when the protective film PF is formed using the substrate processing method of the first embodiment, the formation of the protective film PF is suppressed to a depth of about 0.6 μm below the mask MA when the inhibitor layer IN is used. However, at a position deeper than about 0.6 μm, the protective film PF is formed almost conformally. On the other hand, as shown in FIG. 12(B), when the protective film PF is formed using the substrate processing method of the third embodiment, the thickness of the protective film PF to a depth of about 0.6 μm below the mask MA is suppressed to about half by using the inhibitor layer IN. Furthermore, at a position deeper than about 0.6 μm, the formation of the protective film PF is suppressed as in the case where the inhibitor layer IN is not used. In this way, by using the inhibitor layer IN, the film thickness of the protective film PF above the recess can be further finely suppressed. Furthermore, the difference in film thickness of the protective film PF in the depth direction of the recess can be maintained.

[0107] FIG. 15 is a diagram showing an example of a cross section of a recess after processing. In the recess in the initial state, the opening dimension near the upper part of the mask MA is about 45 nm, as shown in FIG. 15(A), for example. In contrast, when the protective film PF is formed using the substrate processing method in the first embodiment (Reference Example 1), the opening dimension is reduced to about 30 nm, as shown in FIG. 15(B), for example. On the other hand, when the inhibitor layer IN is formed and then the protective film PF is formed using the substrate processing method in the first embodiment by normal ALD (Reference Example 2), the opening dimension is maintained at about 42 nm, as shown in FIG. 15(C), for example. In contrast, when the protective film PF is formed using the substrate processing method in the second embodiment (Second embodiment), the opening dimension is about 21 nm, as shown in FIG. 15(D), for example. On the other hand, when the inhibitor layer IN is formed using the substrate processing method in the third embodiment and then the protective film PF is formed using the substrate processing method in the second embodiment (Third embodiment), the opening dimension is maintained at about 40 nm, as shown in FIG. 15(E), for example. In this way, the use of the inhibitor layer IN to suppress the formation of the protective film PF near the upper portion of the mask MA was found to have the effect of preventing the opening of the recess from being blocked.

[0108] Furthermore, in the third embodiment, the protective film PF can be formed at any position by adjusting the formation position of the inhibitor layer IN. Therefore, the protective film PF can be formed at a desired position while adjusting the film thickness of the protective film PF according to the shape abnormality of the pattern that is expected to occur, such as bowing and necking. In addition, the film formation position on the side wall of the recess can be adjusted by making the formation position of the inhibitor layer IN dependent on A / R. In addition, by changing the composition of the inhibitor layer IN, it is possible to inhibit either the adsorption of the precursor P or the adsorption of the reaction gas R in ALD. For example, if an inhibitor layer IN containing carbon is formed, the oxidation of the precursor P can be inhibited, and if an inhibitor layer IN containing CF is formed, the adsorption of the precursor P can be inhibited.

[0109] (Fourth embodiment) In the second and third embodiments described above, the protective film PF is formed by changing the coverage rate in the depth direction of the recesses with a high A / R. In contrast, in this embodiment, the protective film PF can be formed not only on recesses with a high A / R but also on recesses with a low A / R, such as recesses with an A / R of less than 5, by changing the coverage rate in the depth direction of the recesses. In the following description, "low A / R" refers to an A / R of less than 5, for example.

[0110] (Substrate processing method) Fig. 16 is a flow chart showing an example of a substrate processing method in the fourth embodiment. In this embodiment, a protective film PF is formed on a side wall of a recess by the same method as the substrate processing method illustrated in Fig. 1, except for the points described below. Also in this embodiment, the substrate W is processed by the substrate processing system 1 described with reference to Figs. 4 to 6. In this embodiment, a measuring device for measuring the A / R of the recess is provided in the storage chamber 15 of the substrate processing system 1 illustrated in Fig. 4.

[0111] In this embodiment, first, the processes of steps S10 to S13 illustrated in Fig. 1 are performed. As a result, a recess is formed in the film EL, for example, as shown in Fig. 17(A). Then, the substrate W is carried into the storage chamber 15, and the A / R of the recess is measured. The method for measuring the A / R of the recess is not particularly limited, and may be, for example, an optical method.

[0112] Then, the control device 100 judges whether the measured A / R of the recess is equal to or greater than a predetermined value (S50). If the A / R of the recess is less than the predetermined value (S50: No), the substrate W is carried into the film forming device 14. Then, as shown in FIG. 17(B), for example, a preliminary film PC is formed on the upper part of the recess (S51). At this time, the protective film PF is mainly formed on the upper part of the recess, and the protective film PF is formed on the lower part and bottom of the recess using processing conditions that make it difficult to form the protective film PF. Then, the substrate W is carried into the storage chamber 15 again, and the processing shown in step S50 is performed.

[0113] On the other hand, if A / R of the recess is equal to or greater than the predetermined value (S50: Yes), the processes of steps S14 to S22 illustrated in FIG. 1 are executed. For example, a protective film PF is formed on the top of the recess by the processes of steps S14 to S17, as shown in FIG. 17(C). Then, the bottom of the recess is further etched by the processes of steps S18 to S21, as shown in FIG. 17(D). Then, the substrate W is unloaded by step S22, and the protective film PF is removed by a removal device (not shown). As a result, the cross section of the recess becomes, for example, as shown in FIG. 17(E).

[0114] Fifth embodiment When etching is performed, the depth of the recess formed in the film EL increases and the thickness of the mask MA decreases. The protective film PF is formed near the boundary between the mask MA and the film EL where shape abnormalities are likely to occur, thereby suppressing shape abnormalities of the recess. However, if the thickness of the mask MA changes as etching progresses, the distance between the top of the mask MA and the boundary between the mask MA and the film EL changes. If the protective film PF is continuously formed under conditions in which the protective film PF is formed at the boundary between the mask MA and the film EL according to the thickness of the mask MA before the start of etching, the position where the protective film PF is formed will shift from the boundary between the mask MA and the film EL as etching progresses. Therefore, in this embodiment, the processing conditions for forming the protective film PF are changed according to the thickness of the mask MA. As a result, shape abnormalities of the recess can be suppressed even if etching progresses.

[0115] (Substrate processing method) Fig. 18 is a flow chart showing an example of a substrate processing method in the fifth embodiment. In this embodiment, a protective film PF is formed on a side wall of a recess by the same method as the substrate processing method illustrated in Fig. 1, except for the points described below. Also in this embodiment, the substrate W is processed by the substrate processing system 1 described with reference to Figs. 4 to 6. In this embodiment, a measuring device for measuring the shape of the recess is provided in the storage chamber 15 of the substrate processing system 1 illustrated in Fig. 4. The measuring device in this embodiment is an example of the first measuring device.

[0116] In this embodiment, first, the processes of steps S10 to S13 illustrated in Fig. 1 are performed. As a result, a recess is formed in the film EL, for example, as shown in Fig. 19(A). Then, the substrate W is carried into the storage chamber 15, and the shape of the recess is measured by a measuring device (S60). The shape of the recess is, for example, the A / R of the recess.

[0117] Then, the control device 100 judges whether the shape of the measured recess is a predetermined shape (S61). The predetermined shape is, for example, a shape in which the A / R of the recess is equal to or greater than a predetermined value. If the shape of the recess is a predetermined shape (S61: Yes), the process shown in step S22 is executed.

[0118] On the other hand, if the shape of the recess is not a predetermined shape (S61: No), the thickness of the mask MA is measured by the measuring device. Then, the control device 100 determines whether the thickness of the mask MA is equal to or greater than a predetermined thickness (S62). If the thickness of the mask MA is equal to or greater than a predetermined thickness (S62: Yes), the processes shown in steps S14 to S21 are executed, and the process shown in step S60 is executed again.

[0119] By the processes shown in steps S14 to S17, a protective film PF is formed on the top of the recessed portion, as shown in Fig. 19(B), for example. Then, by the processes in steps S18 to S21, the bottom of the recessed portion is further etched, as shown in Fig. 19(C), for example. This reduces the thickness of the mask MA, as shown in Fig. 19(C).

[0120] On the other hand, if the thickness of the mask MA is less than the predetermined thickness (S62: No), the control device 100 resets the process conditions for forming the protective film PF (S63). Then, the processes shown in steps S14 to S21 are performed based on the reset process conditions. The reset process conditions are, for example, process conditions under which the protective film PF is formed near the boundary between the mask MA and the film EL at the current thickness of the mask MA. This makes it possible to form the protective film PF near the boundary between the mask MA and the film EL even if the thickness of the mask MA decreases as etching progresses, and makes it possible to suppress shape abnormalities in the recesses. The reset process conditions may be etching conditions for the recesses.

[0121] In addition, in this embodiment, the processing conditions of the processing shown in steps S14 to S21 are changed depending on whether the thickness of the mask MA is equal to or greater than a predetermined thickness, but the disclosed technology is not limited to this. As another embodiment, when the processing of steps S14 to S21 is repeated n times (n is an integer equal to or greater than 2) or more, the deposition conditions of the nth protective film PF may be changed from the deposition conditions of the (n-1)th protective film PF depending on the shape of the recess, regardless of the thickness of the mask MA. Alternatively, when the processing of steps S14 to S21 is repeated n times or more, the deposition conditions of the nth protective film PF may be changed from the deposition conditions of the (n-1)th protective film PF depending on the shape of the recess, regardless of the thickness of the mask MA or the shape of the recess. The deposition conditions to be changed are, for example, processing conditions related to the position of the sidewall of the recess on which the protective film PF is formed and the film thickness of the protective film PF formed on the sidewall of the recess. The etching conditions of the recess may be changed.

[0122] Sixth embodiment In the second embodiment, at least one of the precursor P and the reaction gas R is supplied only to a predetermined portion of the side wall of the recess, so that the reaction between the precursor P and the reaction gas R occurs only in the predetermined portion of the side wall of the recess. In contrast, in the present embodiment, the temperature of the substrate W is controlled to control the range in the depth direction of the recess where the protective film PF is formed.

[0123] (Substrate processing method) Fig. 20 is a flow chart showing an example of a substrate processing method in the sixth embodiment. In this embodiment, a protective film PF is formed on a side wall of a recess by a method similar to the substrate processing method illustrated in Fig. 1, except for the points described below. In this embodiment, the substrate W is processed by the substrate processing system 1 described with reference to Fig. 4, but the protective film PF is formed in each etching apparatus 12. In this embodiment, the electrostatic chuck ESC is divided into a plurality of zones, and the temperature of each zone is individually controlled by a heater HT.

[0124] In this embodiment, first, the processes of steps S10 to S13 illustrated in Fig. 1 are performed. Then, in the etching apparatus 12, the temperature of the substrate W is adjusted to 200°C or higher, and at least two zones of the electrostatic chuck ESC are set to different temperatures (S70). Then, the processes of steps S16 to S22 are performed. Note that in this embodiment, the processes of S16 to S17 are performed in each etching apparatus 12, and the process of step S18 is not performed.

[0125] In this embodiment, the electrostatic chuck ESC of the etching apparatus 12 is divided into a plurality of concentric zones Z1 to Z3 as shown in Fig. 21. The temperature of each of the zones Z1 to Z3 is individually controlled by a heater HT. The manner of dividing the plurality of zones whose temperatures can be individually controlled is not limited to that shown in Fig. 21. As another example, the electrostatic chuck ESC of the etching apparatus 12 may be divided into 14 zones Z1 to Z14 as shown in Figs. 22 and 23.

[0126] (Relationship between temperature and deposition position of protective film PF) FIG. 24 is a diagram showing an example of CD distribution in the depth direction of the recess under a first temperature condition. FIG. 25 is a diagram showing an example of CD distribution in the depth direction of the recess under a second temperature condition. In the experimental results shown in FIG. 24 and FIG. 25, a process consisting of four steps of introduction of precursor P, purging, introduction of reactive gas R, and purging was performed 35 times. In the introduction of reactive gas R, the reactive gas R was turned into plasma. The precursor P was a silicon-containing gas, and the reactive gas was oxygen gas diluted with argon. Therefore, the protective film PF formed in FIG. 24 and FIG. 25 is a silicon oxide film. It is considered that the film formation characteristics of the silicon oxide film with respect to temperature are similar to the film formation characteristics of the silicon nitride film with respect to temperature. Therefore, the following will be described by taking the protective film PF as a silicon oxide film as an example.

[0127] In the experiment, the temperature of the electrostatic chuck ESC when introducing the reactive gas R was set to two types, and the thickness and position of the protective film PF formed were measured. In the experiment of Fig. 24, the temperature of the electrostatic chuck ESC was adjusted to 10°C, and in the experiment of Fig. 25, the temperature of the electrostatic chuck ESC was adjusted to 60°C. In addition, the introduction time of the reactive gas R (plasma generation time) was set to four types: 1 second, 4 seconds, 10 seconds, and saturation completion time (a time sufficient for the reactive gas R to complete saturation on the surface of the substrate W).

[0128] 24 and 25, "Initial" shows the CD of the recess before the experiment started, and "Conformal" shows the CD of the recess when the treatment was continued until the saturation completion time. As can be seen from Fig. 24 and Fig. 25, in the "Conformal" case, a protective film PF is formed on the side wall of the recess with a nearly uniform thickness regardless of the depth of the recess.

[0129] Next, the thickness of the protective film PF formed in the recess was measured by changing the introduction time of the reaction gas R. As can be seen from the graph in FIG. 24, the state of the protective film PF formed when the introduction time of the reaction gas R is set to 10 seconds is a state in which the film thickness decreases slightly toward the bottom of the recess, but the film thickness is almost conformal. In addition, when the introduction time of the reaction gas R is set to 4 seconds, the thickness of the protective film PF formed is different compared to the case of 10 seconds, and a thinner protective film PF is formed at the bottom of the side wall of the recess compared to the case of 10 seconds. When the introduction time of the reaction gas R is set to 1 second, a protective film PF whose thickness gradually decreases in the depth direction of the recess is formed from the boundary between the mask MA and the film EL to a position about 0.6 μm in the depth direction of the recess. However, the protective film PF is hardly formed in the part below 0.6 μm.

[0130] On the other hand, looking at the graph of FIG. 25 in which the temperature of the electrostatic chuck ESC is adjusted to 60° C., the state of the protective film PF formed when the introduction time of the reaction gas R is set to 10 seconds is almost conformal, although the film thickness decreases slightly downward. When the introduction time of the reaction gas R is set to 4 seconds, the thickness of the protective film PF formed differs from that in the case of 10 seconds, and a thinner protective film PF is formed at the lower part of the side wall of the recess compared to the case of 10 seconds. When the introduction time of the reaction gas R is set to 1 second, a protective film PF whose thickness gradually decreases in the depth direction of the recess is formed from the boundary between the mask MA and the film EL to a position about 1 μm in the depth direction of the recess. However, almost no protective film PF is formed below 1 μm.

[0131] When the introduction time of the reaction gas R is shortened in either case, a protective film PF is formed whose thickness gradually decreases in the depth direction of the recess. In particular, when the introduction time of the reaction gas R is set to 1 second, the formation of the protective film PF at a position below 0.6 μm can be suppressed if the temperature of the electrostatic chuck ESC is controlled to 10° C., and the formation of the protective film PF at a position below 1 μm can be suppressed if the temperature of the electrostatic chuck ESC is controlled to 60° C. In this way, it can be seen from the experimental results shown in FIG. 24 and FIG. 25 that the thickness of the protective film PF formed and the distribution of the protective film PF can be adjusted by changing the temperature of the electrostatic chuck ESC.

[0132] Figure 26 is a diagram summarizing the experimental results of Figures 24 and 25. Specifically, Figure 26 was obtained by superimposing the experimental results on a graph showing the correspondence between the saturation time of oxygen (O2) plasma and A / R, which is calculated using a diffusion equation or the like.

[0133] As shown in Fig. 26, the lower limit position (A / R) at which the film is formed changes in response to a change in the introduction time of the reactive gas R (here, the irradiation time of O2 plasma). In addition, when the temperature of the electrostatic chuck ESC is set to 10°C and when it is set to 60°C, there is a difference of about 20 in A / R in the lower limit position at which the protective film PF is formed (part indicated by the arrow in Fig. 26). From this, by varying the temperature of the electrostatic chuck ESC within a range of, for example, 10°C to 60°C, it is possible to vary the lower limit position at which the protective film PF is formed within a range of A / R of about 20.

[0134] For this reason, in this embodiment, the position of the sidewall of the recess where shape abnormalities such as bowing or taper occur is observed in advance, and then the protective film PF is formed in the region of the sidewall where the shape abnormality is likely to occur. Also, in this embodiment, the temperature of the electrostatic chuck ESC on which the substrate W is placed is adjusted to adjust the deposition region of the protective film PF on the sidewall of the recess. Also, in this embodiment, by forming the protective film PF whose film thickness gradually decreases in the depth direction of the recess, the protective film PF can be formed in the region (position) corresponding to the shape abnormality of the recess such as taper or bowing.

[0135] Seventh embodiment In this embodiment, after the processes of steps S10 to S21 in FIG. 1 are performed, the substrate W is loaded into the storage chamber 15. A measuring device provided in the storage chamber 15 measures the state of the protective film PF formed in the recess. The measuring device provided in the storage chamber 15 is an example of a second measuring device. The state of the protective film PF to be measured is, for example, the film thickness of the protective film PF and the position on the side wall of the recess where the protective film PF remains. Then, the control device 100 determines whether the state of the protective film PF is in a predetermined state or not according to the measured state of the protective film PF.

[0136] If the state of the protective film PF is in a predetermined state, the processes of steps S14 to S21 are continuously performed one or more times until a recess having a predetermined shape is formed. On the other hand, if the state of the protective film PF is not in a predetermined state, the control device 100 adjusts at least a part of the process conditions in the processes of steps S14 to S21 based on the measured state of the protective film PF so that the state of the protective film PF becomes a predetermined state. Then, the processes of steps S14 to S21 are performed one or more times.

[0137] [others] It should be noted that the technology disclosed in the present application is not limited to the above-described embodiment, and various modifications are possible within the scope of the gist thereof.

[0138] For example, in each of the above-mentioned embodiments, the formation of the protective film PF, which is a silicon nitride film, on the sidewall of the recess and the further etching of the recess are repeated, but the disclosed technology is not limited to this. For example, the substrate W shown in FIG. 27(A) is etched to form the recess shown in FIG. 27(B), and the protective film PF1, which is a silicon nitride film, is formed on the sidewall of the recess as shown in FIG. 27(C). Then, after the recess is further etched as shown in FIG. 27(D), a protective film PF2, which is, for example, a silicon oxide film, may be formed on the sidewall of the recess as shown in FIG. 27(E). Then, the recess is further etched as shown in FIG. 27(F). In this way, while the formation of the protective film PF and the etching of the recess are repeated, the protective film PF2, which is a silicon oxide film, may be formed at least once as the protective film PF. The protective film PF2 is an example of a third film. The silicon oxide film can be formed under a lower temperature condition than the silicon nitride film. Therefore, the protective film PF1 can be formed under temperature conditions close to those in which etching is performed. This allows the protective film PF1 to be formed within the etching apparatus 12. This allows the time required to transport the substrate W between the etching apparatus 12 and the film forming apparatus 14 to be reduced, thereby improving throughput.

[0139] It should be noted that the embodiments disclosed herein are illustrative in all respects and should not be construed as limiting. Indeed, the above-described embodiments may be embodied in various forms. Furthermore, the above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. [Explanation of symbols]

[0140] EL membrane I Inhibitor IN Inhibitor layer MA Mask P Precursor PC spare film PF protective film R Reactive gas W substrate 1. Substrate Processing System 100 Control device 12 Etching equipment 13 Vacuum transfer chamber 14 Film deposition equipment 15 Storage room 16 Load lock chamber 17 Atmospheric Transfer Chamber

Claims

1. a) carrying into a first chamber a substrate having a first film to be processed, the first film having a recess formed therein, and a mask provided on the first film and having an opening formed at a position corresponding to the recess; b) adjusting the temperature of the substrate to 200° C. or higher; c) forming a second film, which is a silicon nitride film, on a side wall of the recess; d) loading the substrate into a second chamber different from the first chamber; e) adjusting the temperature of the substrate to 100° C. or less; f) etching the bottom of the recess while protecting the sidewalls of the recess with the second film; Including, The c) is c-1) supplying a silicon-containing reactive species into the first chamber to adsorb the silicon-containing reactive species on a sidewall of the recess; c-2) supplying a nitrogen-containing reactive species into the first chamber and reacting the silicon-containing reactive species adsorbed on the sidewall of the recess with the nitrogen-containing reactive species, thereby forming the second film on the sidewall of the recess; Including, The second film has a thickness of 20 nm or less, the second film has a ratio of a film thickness at a bottom of the recess to a film thickness at an upper sidewall of the recess of 0.7 or less; a) performing the steps a) to f) in this order at least twice until an aspect ratio, which is a ratio of a depth dimension from an opening of the mask to a bottom of the recess to a dimension of the opening of the mask, becomes 50 or more.

2. The method further includes, before the step a), etching the first film through the mask to form the recess; Before the step of forming the recess is performed, the mask has a thickness of 2000 nm or more; The substrate processing method of claim 1 , wherein the mask has an aspect ratio of 20 or more.

3. 3. The substrate processing method according to claim 1, wherein in the substrate carried in at step a), a ratio of a depth dimension from an upper portion of the mask to a bottom portion of the recess to a dimension of the opening of the mask is 10 or more.

4. 4. The substrate processing method according to claim 1, wherein after repeating steps a) to f) two or more times until the aspect ratio becomes 50 or more, a ratio of a depth dimension from an upper portion of the mask to a bottom of the recess to a dimension of an opening of the mask is 10 or less.

5. The substrate processing method according to claim 1 , wherein the nitrogen-containing reactive species is generated by converting a nitrogen-containing gas into plasma.

6. The c) is c-0) A step of terminating the surface of the substrate with amino groups by generating plasma of a gas containing nitrogen and hydrogen in the first chamber. Including, The substrate processing method according to claim 1 , wherein the step c-0) is performed before the step c-1).

7. The substrate processing method according to claim 1 , wherein in the step c), the second film is formed on a side wall of the recess with a thickness of 10 nm or less.

8. a mask film is provided on the substrate on the first film; In the step c), the second film is also formed on the surface of the mask film; The substrate processing method according to claim 1 , wherein a thickness of the second film formed on a side wall of the mask film is greater than a thickness of the second film formed on a surface of the recess.

9. 9. The substrate processing method according to claim 1, wherein in the step c-2), a bias voltage is applied to a lower electrode constituting a mounting table on which the substrate is placed.

10. the first film includes a silicon oxide film and a silicon nitride film; 10. The substrate processing method according to claim 1, wherein the silicon nitride film included in the first film and the second film have different content ratios of silicon atoms and nitrogen atoms.

11. the first film includes a silicon oxide film and a silicon nitride film; The substrate processing method according to claim 1 , wherein the silicon nitride film of the first film and the second film have different film densities.

12. the first film includes a silicon oxide film and a silicon nitride film; The substrate processing method according to claim 1 , wherein the silicon nitride film of the first film and the second film have different crystal structures.

13. The substrate processing method according to claim 1 , wherein at least one of a time period during which the silicon-containing reactive species is supplied and a time period during which the nitrogen-containing reactive species is supplied is made longer as the aspect ratio increases.

14. The substrate processing method includes: a batch-type film forming apparatus capable of accommodating a plurality of the substrates; Multiple single-wafer etching equipment The method is carried out using a substrate processing system comprising: the first chamber is the film forming apparatus, The substrate processing method according to claim 1 , wherein the second chamber is an etching apparatus.

15. g) forming a third film, which is a silicon oxide film, on a side wall of the recess formed in the step f) in a third chamber; The step g) is performed after the step f); The substrate processing method according to claim 1 , further comprising the step f) being performed after the step g) is performed.

16. The substrate processing method of claim 15 , wherein the second chamber and the third chamber are the same chamber.

17. h) providing a substrate having a recess formed in a first film; i) adjusting the temperature of the substrate to 200° C. or higher; j) forming a second film, which is a silicon nitride film, on a side wall of the recess; k) etching the bottom of the recess while protecting the sidewall of the recess with the second film; A method for processing a substrate, comprising:

18. a first chamber for accommodating a substrate having a recess formed in a first film to be processed; a first temperature adjustment unit that adjusts a temperature of the substrate accommodated in the first chamber; a first gas supply unit that supplies a gas into the first chamber; a second chamber that houses the substrate and is different from the first chamber; a second temperature adjustment unit that adjusts the temperature of the substrate accommodated in the second chamber; a second gas supply unit that supplies a gas into the second chamber; a transfer device that transfers the substrate between the first chamber and the second chamber; Control device and Equipped with The control device includes: a) controlling the transfer device to load the substrate into the first chamber; b) controlling the first temperature adjustment unit so that the temperature of the substrate is 200° C. or higher; c) controlling the first gas supply unit to deposit a second film, which is a silicon nitride film, on a side wall of the recess; d) controlling the transfer device to transfer the substrate into the second chamber; e) controlling the second temperature adjustment unit so that the temperature of the substrate is 100° C. or less; f) controlling the second gas supply unit so as to etch the bottom of the recess while protecting the sidewall of the recess with the second film; A substrate processing system.

19. the first chamber is a batch-type film forming apparatus capable of accommodating a plurality of the substrates, 20. The substrate processing system of claim 18, wherein the second chamber is a single wafer etching apparatus.

20. The conveying device is a first transfer device configured to transfer the substrate into the first chamber and to transfer the substrate out of the first chamber; a second transfer device that transfers the substrate into the second chamber and transfers the substrate out of the second chamber; having The substrate processing system of claim 19 , wherein the first transport device is capable of transporting the substrate in a vertical direction.

21. a first measuring device for measuring a shape of the recess; The control device includes:

21. The substrate processing system according to claim 18, wherein at least one of conditions for forming the second film and conditions for etching the bottom of the recess is changed based on the shape of the recess measured by the first measuring device.

22. a second measuring device for measuring a state of the second film; The control device includes:

22. The substrate processing system according to claim 18, wherein at least one of conditions for forming the second film and conditions for etching the bottom of the recess is changed based on the state of the second film measured by the second measuring device.

23. The substrate processing system according to claim 18 , further comprising a storage chamber for storing the substrate on which step c) has been performed, after step c) has been performed, until step d) is started.

Citation Information

Patent Citations

  • Plasma nitriding method

    JP2012216631A

  • Substrate processing system and substrate processing method

    JP2016021546A

  • Etching treatment method

    JP2016207840A

  • Plasma processing apparatus and plasma processing method

    JP2019207913A

  • Substrate processing method and substrate processing device

    JP2020145404A