By applying controlled tension and utilizing a magnetic tape with specific surface features, the magnetic tape device ensures stable running and accurate data recording/reproduction, addressing deformation and misalignment issues for long-term data storage.

JP7565787B2Active Publication Date: 2024-10-11FUJIFILM CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020214224
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-23
Publication Date
2024-10-11
Estimated Expiration
2040-12-23

AI Technical Summary

Technical Problem

Magnetic tapes in magnetic tape devices experience deformation during storage, leading to misalignment of the magnetic head, overwriting of data, and potential damage to the tape edges due to unstable running conditions, which is exacerbated by the need for long-term data archiving.

Method used

The magnetic tape is run with a tension of 0.50N or more in the longitudinal direction between reels and wound onto the cartridge reel with a tension of 0.40N or less, featuring a magnetic layer with specific surface depressions and a non-magnetic support containing ferromagnetic powder, along with a magnetic tape device that controls tension and uses servo patterns for precise tracking.

Benefits of technology

This approach stabilizes the magnetic tape's running, prevents data misalignment and edge damage, ensuring stable recording and playback after storage, particularly suitable for long-term data archiving.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007565787000011
    Figure 0007565787000011
  • Figure 0007565787000012
    Figure 0007565787000012
  • Figure 0007565787000013
    Figure 0007565787000013
Patent Text Reader

Abstract

To provide means that enables stable running of a magnetic tape when accommodating the magnetic tape into a magnetic tape cartridge, and enables proper recording and / or reproduction when recording and / or reproducing data to / from the magnetic tape that has been stored.SOLUTION: A magnetic tape device provided herein is configured to make a magnetic tape to run between a take-up reel and a cartridge reel with a tension applied to the magnetic tape in a longitudinal direction, the maximum tension being 0.50 N or greater, and reel in the magnetic tape after being run with the tension applied thereto to the cartridge reel with a tension of 0.40 N or less applied thereto in the longitudinal direction, and has the number of recesses of 10 to 500 per area of 40×40 μm with circle-equivalent diameters of 0.20 or greater and 0.50 μm or less present on a surface of a magnetic layer of the magnetic tape. The magnetic tape and the magnetic tape cartridge are also disclosed herein.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetic tape device, a magnetic tape, and a magnetic tape cartridge. [Background technology]

[0002] Magnetic recording media include tape-type and disk-type recording media, and tape-type magnetic recording media, that is, magnetic tapes, are primarily used for data storage applications such as data backup and archiving (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6590102 specification Summary of the Invention [Problem to be solved by the invention]

[0004] Data is usually recorded on a magnetic tape by running the magnetic tape in a magnetic tape device (usually called a "drive") and recording data on the data band by making a magnetic head follow the data band of the magnetic tape. This forms a data track on the data band. When playing back recorded data, the magnetic tape is run in the magnetic tape device and the magnetic head follows the data band of the magnetic tape to read the data recorded on the data band. After such recording or playback, the magnetic tape is wound on a reel (hereinafter referred to as a "cartridge reel") in a magnetic tape cartridge and stored until the next recording and / or playback is performed.

[0005] After the above storage, when recording and / or reproducing is performed, if the magnetic head for recording and / or reproducing data deviates from the target track position due to deformation of the magnetic tape and performs recording and / or reproducing of data, phenomena such as overwriting of recorded data and reproduction failure may occur. Meanwhile, in the field of data storage, there has been an increasing need in recent years for long-term storage of data, known as archives. However, in general, the longer the storage period, the more likely the magnetic tape is to deform. Therefore, it is expected that there will be an even greater demand in the future for suppressing the occurrence of the above phenomena after storage.

[0006] Furthermore, if the running condition of the magnetic tape is unstable when the magnetic tape is placed into a magnetic tape cartridge for storage, for example, the edge of the magnetic tape may hit a flange that is typically provided on a cartridge reel, causing damage to the edge.

[0007] In view of the above, one aspect of the present invention aims to provide a means for enabling a magnetic tape to run stably when the magnetic tape is stored in a magnetic tape cartridge, and for enabling data to be recorded and / or reproduced satisfactorily on the magnetic tape after storage. [Means for solving the problem]

[0008] One aspect of the present invention is A take-up reel; A magnetic tape; a magnetic tape cartridge having a cartridge reel; A magnetic tape device comprising: The magnetic tape device is The magnetic tape is run between the take-up reel and the cartridge reel under tension in the longitudinal direction of the magnetic tape, the maximum value of the tension being 0.50 N or more; After the magnetic tape has been run under the above tension, the magnetic tape is wound around the cartridge reel under a tension of 0.40 N or less in the longitudinal direction of the magnetic tape. The magnetic tape has a non-magnetic support and a magnetic layer containing a ferromagnetic powder, a magnetic tape device, in which the number of depressions having a circle equivalent diameter of 0.20 μm or more and 0.50 μm or less present on the surface of the magnetic layer is 10 to 500 per area of ​​40 μm × 40 μm; Regarding.

[0009] Another aspect of the present invention is Between the take-up reel and the cartridge reel of the magnetic tape cartridge, the magnetic tape is run under tension in the longitudinal direction of the magnetic tape, and the maximum value of this tension is 0.50 N or more, and A magnetic tape used in a magnetic tape device that applies a tension of 0.40 N or less in the longitudinal direction of the magnetic tape to the magnetic tape after the magnetic tape has been run under the above-mentioned tension, and winds the magnetic tape around the above-mentioned cartridge reel, A non-magnetic support and a magnetic layer containing ferromagnetic powder, a magnetic tape in which the number of depressions having an equivalent circle diameter of 0.20 μm or more and 0.50 μm or less present on the surface of the magnetic layer is 10 to 500 per 40 μm×40 μm area; Regarding.

[0010] In one embodiment, the tension applied to the magnetic tape in the longitudinal direction during the running can be changed.

[0011] In one embodiment, the magnetic tape may have a tape thickness of 5.2 μm or less.

[0012] In one embodiment, the magnetic tape can further include a non-magnetic layer containing non-magnetic powder between the non-magnetic support and the magnetic layer.

[0013] In one embodiment, the magnetic tape can further have a backcoat layer containing a nonmagnetic powder on the surface side of the nonmagnetic support opposite to the surface side having the magnetic layer.

[0014] In one embodiment, the non-magnetic powder of the backcoat layer can include carbon black.

[0015] In one embodiment, the squareness ratio of the magnetic tape in the perpendicular direction can be 0.60 or more.

[0016] One aspect of the present invention relates to a magnetic tape cartridge in which the above-mentioned magnetic tape is wound around a cartridge reel. Effect of the Invention

[0017] According to one aspect of the present invention, it is possible to allow the magnetic tape to run stably when the magnetic tape is stored in a magnetic tape cartridge, and it is also possible to perform good recording and / or playback of data on the magnetic tape after storage. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a schematic diagram illustrating an example of a magnetic tape device. [Diagram 2] 2 shows an example of the arrangement of data bands and servo bands. [Diagram 3] An example of servo pattern arrangement on an LTO (Linear Tape-Open) Ultrium format tape is shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The magnetic tape device and the magnetic tape will be described in more detail below. In the following, one embodiment of the magnetic tape device and the magnetic tape may be described with reference to the drawings. However, the magnetic tape device and the magnetic tape are not limited to the embodiment shown in the drawings.

[0020] [Magnetic tape device configuration] A magnetic tape device 10 shown in FIG. 1 controls a recording / reproducing head unit 12 in response to commands from a control device 11, and records and reproduces data on a magnetic tape MT. The magnetic tape device 10 has a configuration capable of detecting and adjusting tension applied in the longitudinal direction of the magnetic tape from spindle motors 17A, 17B that control the rotation of the cartridge reel 130 and take-up reel 16 and their drive devices 18A, 18B. The magnetic tape device 10 has a configuration in which a magnetic tape cartridge 13 can be mounted. The magnetic tape device 10 has a cartridge memory read / write device 14 capable of reading from and writing to a cartridge memory 131 in the magnetic tape cartridge 13 . From the magnetic tape cartridge 13 attached to the magnetic tape device 10, the end or leader pin of the magnetic tape MT is pulled out by an automatic loading mechanism or manually, and the magnetic tape MT passes over the recording / playback head via guide rollers 15A and 15B with the magnetic layer surface in a direction facing the recording / playback head surface of the recording / playback head unit 12, and the magnetic tape MT is wound onto the take-up reel 16. The rotation and torque of spindle motors 17A and 17B are controlled by signals from control device 11, and magnetic tape MT runs at any speed and tension. A servo pattern formed in advance on the magnetic tape can be used to control the tape speed. A tension detection mechanism may be provided between magnetic tape cartridge 13 and take-up reel 16 to detect the tension. The tension may be adjusted using guide rollers 15A and 15B in addition to the control by spindle motors 17A and 17B. The cartridge memory read / write device 14 is configured to be able to read and write information from and to the cartridge memory 131 in response to commands from the control device 11. As a communication method between the cartridge memory read / write device 14 and the cartridge memory 131, for example, the ISO (International Organization for Standardization) 14443 method can be adopted.

[0021] The control device 11 includes, for example, a control unit, a storage unit, a communication unit, and the like.

[0022] The recording and reproducing head unit 12 is composed of, for example, a recording and reproducing head, a servo tracking actuator that adjusts the position of the recording and reproducing head in the track width direction, a recording and reproducing amplifier 19, a connector cable for connecting to the control device 11, etc. The recording and reproducing head is composed of, for example, a recording element that records data on the magnetic tape, a reproducing element that reproduces the data on the magnetic tape, and a servo signal reading element that reads the servo signal recorded on the magnetic tape. One magnetic head is equipped with, for example, one or more of each of the recording element, reproducing element, and servo signal reading element. Alternatively, each element may be provided separately in a plurality of magnetic heads according to the running direction of the magnetic tape.

[0023] The recording / reproducing head unit 12 is configured to be capable of recording data onto the magnetic tape MT in response to a command from the control device 11. Also, the recording / reproducing head unit 12 is configured to be capable of reproducing the data recorded onto the magnetic tape MT in response to a command from the control device 11.

[0024] The control device 11 has a mechanism for determining the running position of the magnetic tape MT from the servo signal read from the servo band while the magnetic tape MT is running, and for controlling the servo tracking actuator so that the recording element and / or the reproducing element are positioned at the target running position (track position). This control of the track position is performed, for example, by feedback control. The control device 11 has a mechanism for determining the servo band interval from the servo signals read from two adjacent servo bands while the magnetic tape MT is running. The control device 11 also has a mechanism for adjusting and changing the tension applied to the magnetic tape in the longitudinal direction by controlling the torque of the spindle motor 17A and the spindle motor 17B and / or the guide rollers 15A and 15B so that the servo band interval becomes a target value. This tension adjustment is performed by, for example, feedback control. The control device 11 can also store information on the determined servo band interval in a storage unit inside the control device 11, a cartridge memory 131, an external connected device, or the like.

[0025] In the above magnetic tape device, the tension applied in the longitudinal direction of the magnetic tape during recording and / or playback is a constant value in one embodiment, and varies in another embodiment. In the present invention and this specification, the value of the tension applied in the longitudinal direction of the magnetic tape is the tension value used by the control device of the magnetic tape device to control the mechanism for adjusting the above tension as the tension to be applied in the longitudinal direction of the magnetic tape. Furthermore, the tension actually applied in the longitudinal direction of the magnetic tape in the magnetic tape device can be detected, for example, by providing a tension detection mechanism between the magnetic tape cartridge 13 and the take-up reel 16 in FIG. 1, as described above. Furthermore, for example, the minimum tension can be controlled by the control device of the magnetic tape device so that it does not fall below a value or a recommended value set by a standard, etc., and / or the maximum tension does not exceed a value or a recommended value set by a standard, etc.

[0026] [Magnetic tape cartridge] Before being loaded into a magnetic tape device and after being removed from the magnetic tape device, a magnetic tape cartridge generally contains a magnetic tape wound around a cartridge reel inside the cartridge body. The cartridge reel is rotatably provided inside the cartridge body. As magnetic tape cartridges, single-reel type magnetic tape cartridges having one reel inside the cartridge body and twin-reel type magnetic tape cartridges having two reels inside the cartridge body are widely used. The magnetic tape cartridge included in the magnetic tape device can be a single-reel type magnetic tape cartridge in one form, and can be a twin-reel type magnetic tape cartridge in another form. In the case of a twin-reel type magnetic tape cartridge, the cartridge reel refers to the reel on which the magnetic tape is mainly wound when it is stored after data is recorded and / or played back, and the other reel is referred to as the winding reel. When a single-reel magnetic tape cartridge is loaded into a magnetic tape device for recording and / or reproducing data on the magnetic tape, the magnetic tape is pulled out from the magnetic tape cartridge and wound around the take-up reel of the magnetic tape device, as shown in FIG. 1 for example. A magnetic head is disposed on the magnetic tape transport path from the magnetic tape cartridge to the take-up reel. The magnetic tape runs by being fed out and taken up between the cartridge reel (also called the "supply reel") of the magnetic tape cartridge and the take-up reel of the magnetic tape device. During this time, the magnetic head comes into contact with and slides against the magnetic layer surface of the magnetic tape, thereby recording and / or reproducing data. In contrast, a dual-reel magnetic tape cartridge is provided with both a supply reel and a take-up reel inside the magnetic tape cartridge.

[0027] In one embodiment, the magnetic tape cartridge may include a cartridge memory. The cartridge memory may be, for example, a non-volatile memory, in which tension adjustment information is already recorded or tension adjustment information is to be recorded. The tension adjustment information is information for adjusting the tension applied in the longitudinal direction of the magnetic tape. For the cartridge memory, the above description may also be referred to.

[0028] [Tension during running, tension during winding onto cartridge reel] In a magnetic tape device, the magnetic tape is run between a cartridge reel (supply reel) and a take-up reel, and data can be recorded on the magnetic tape and / or the recorded data can be reproduced. In the magnetic tape device, tension is applied in the longitudinal direction of the magnetic tape during the running. The greater the tension applied in the longitudinal direction of the magnetic tape, the greater the shrinkage of the widthwise dimension of the magnetic tape (i.e., the narrower the width can be), and the smaller the tension, the smaller the degree of shrinkage can be. Therefore, the widthwise dimension of the magnetic tape can be controlled by the value of the tension applied in the longitudinal direction of the magnetic tape running in the magnetic tape device. In the magnetic tape device, the magnetic tape runs with a maximum tension of 0.50 N or more applied in the longitudinal direction. If the magnetic tape is stored in a magnetic tape cartridge after running with such a large tension applied, it is considered that the magnetic tape is likely to be deformed during storage. For example, it is presumed that during storage, the magnetic tape housed in a magnetic tape cartridge is deformed such that the portion close to the cartridge reel becomes wider than the initial width due to compressive stress in the tape thickness direction, and the portion far from the cartridge reel becomes narrower than the initial width due to tensile stress in the tape longitudinal direction, and that deformation that differs depending on the position occurs, and it is considered that a magnetic tape housed in a state in which a large tension is applied is likely to have a larger difference in deformation depending on the position. This is considered to be a cause that when recording and / or reproducing is performed after storage, the magnetic head may record and / or reproduce data while shifting from the target track position. Therefore, in the above magnetic tape device, when the magnetic tape is wound onto the cartridge reel after it has been run with a maximum tension of 0.50 N or more applied in the longitudinal direction, the tension applied to the magnetic tape in the longitudinal direction is set to 0.40 N or less. This makes it possible to wind the magnetic tape onto the cartridge reel with a tension smaller than the tension applied in the longitudinal direction during running and store it in the magnetic tape cartridge, and the inventors believe that this makes it possible to suppress the occurrence of the phenomenon that can occur due to the deformation described above. However, the inventors have found in their research that the running state of the magnetic tape is likely to become unstable when a relatively small tension of 0.40 N or less is applied to wind the magnetic tape onto a cartridge reel. In contrast, in the magnetic tape, the number of depressions with a circle equivalent diameter of 0.20 μm to 0.50 μm present on the surface of the magnetic layer is 10 to 500 per area of ​​40 μm × 40 μm. The inventors speculate that this leads to improved running stability when the magnetic tape is wound onto a cartridge reel with a tension of 0.40 N or less.

[0029] In the above magnetic tape device, the maximum value of the tension applied in the longitudinal direction of the magnetic tape during running is 0.50N or more, and can be 0.60N or more, 0.70N or more, or 0.80N or more. The maximum value can be, for example, 1.50N or less, 1.40N or less, 1.30N or less, 1.20N or less, 1.10N or less, or 1.00N or less. The tension applied in the longitudinal direction of the magnetic tape during running can be a constant value or can be changed. In the case of a constant value, the tension applied in the longitudinal direction of the magnetic tape can be controlled, for example, by a control device of the magnetic tape device, so that a constant value of tension of 0.50N or more is applied in the longitudinal direction of the magnetic tape. On the other hand, when the tension applied in the longitudinal direction of the magnetic tape during running is changed, for example, a servo signal can be used to obtain dimensional information in the width direction of the magnetic tape during running, and the tension applied in the longitudinal direction of the magnetic tape can be adjusted and changed according to the obtained dimensional information. This makes it possible to control the dimension in the width direction of the magnetic tape. One form of such tension adjustment has been described above with reference to FIG. 1. However, the magnetic tape device is not limited to the embodiment shown in the example. In the magnetic tape device, when the tension applied in the longitudinal direction of the running magnetic tape is changed, the minimum value can be, for example, 0.10 N or more, 0.20 N or more, 0.30 N or more, or 0.40 N or more. In one embodiment, the minimum value can be, for example, 0.40 N or less or less than 0.40 N, and in another embodiment, 0.60 N or less or 0.50 N or less.

[0030] In a magnetic tape device, when a magnetic tape is run for recording and / or reproducing data, the following specific modes of running the magnetic tape can be given. Type 1: At the end of a run for recording and / or reproducing data, the entire length of the magnetic tape is wound onto the take-up reel. Type 2: At the end of a run for recording and / or reproducing data, the entire length of the magnetic tape is wound onto the cartridge reel. Mode 3: At the end of running for recording and / or reproducing data, a portion of the magnetic tape is wound on the cartridge reel and a portion is wound on the take-up reel.

[0031] In the first embodiment, the tension applied in the longitudinal direction of the magnetic tape when the entire length of the magnetic tape is wound onto a cartridge reel to be housed in a magnetic tape cartridge is 0.40 N or less. In the second embodiment, the magnetic tape is first wound from the cartridge reel onto the take-up reel. The tension applied to the magnetic tape in the longitudinal direction at this time is not particularly limited. It may be a constant value or may be variable, and may or may not conform to the above description regarding the tension value during running. If the tension applied to the magnetic tape in the longitudinal direction when it is subsequently wound onto the cartridge reel is 0.40 N or less, data can be recorded and / or reproduced satisfactorily when recording and / or reproducing data on the magnetic tape after storage. The tension applied to the magnetic tape in the longitudinal direction when the entire length of the magnetic tape is wound from the take-up reel onto the cartridge reel is 0.40 N or less. Form 3 can be either of the following two forms. The first form (form 3-1) is a form in which, at the end of running for recording and / or reproducing data, the portion of the magnetic tape wound around the cartridge reel is wound with a tension of 0.40 N or less in the longitudinal direction when wound around the cartridge reel. The second form (form 3-2) is a form other than form 3-1 of form 3. In form 3-1, in order to wind the entire length of the magnetic tape onto the cartridge reel and accommodate it in the cartridge, the tension applied in the longitudinal direction of the magnetic tape when winding the magnetic tape that is not wound around the cartridge reel onto the cartridge reel is 0.40 N or less. Form 3-2 is the same as form 2. That is, first, the magnetic tape is wound from the cartridge reel onto the take-up reel. Then, the tension applied in the longitudinal direction of the magnetic tape when winding the entire length of the magnetic tape from the take-up reel onto the cartridge reel is 0.40 N or less. In any of the above-mentioned first, second and third embodiments, the tension applied in the longitudinal direction of the magnetic tape when it is wound around the cartridge reel may be a constant value of 0.40 N or less, or may be changed within a range of 0.40 N or less. The maximum value of the tension applied in the longitudinal direction of the magnetic tape when it is wound around the cartridge reel is 0.40 N or less, and may be 0.35 N or less or 0.30 N or less. The minimum value of the tension applied in the longitudinal direction of the magnetic tape when it is wound around the cartridge reel may be, for example, 0.10 N or more, 0.20 N or more, 0.30 N or more, or more than 0.30 N, or may be less than the value exemplified here. The tension when it is wound around the cartridge reel may be controlled, for example, by a control device of the magnetic tape device. Also, an operation program may be recorded in the cartridge memory so that the magnetic tape is wound around the cartridge reel with the rewinding tension set in the longitudinal direction after recording and / or reproducing data on the magnetic tape, and the control device may read out this program to execute the winding operation.

[0032] [Magnetic tape] The magnetic tape device includes a magnetic tape having a non-magnetic support and a magnetic layer containing ferromagnetic powder, in which the number of depressions on the surface of the magnetic layer having a circle equivalent diameter of 0.20 μm or more and 0.50 μm or less is 10 to 500 per area of ​​40 μm x 40 μm.

[0033] <State of depressions on the magnetic layer surface> In the present invention and this specification, the number of recesses having an equivalent circle diameter of 0.20 μm or more and 0.50 μm or less on the surface of the magnetic layer is determined by measuring the surface of the magnetic layer of the magnetic recording medium using an atomic force microscope (AFM) as follows. In the present invention and this specification, the "surface of the magnetic layer" is synonymous with the magnetic layer side surface of the magnetic recording medium. The number of recesses having an equivalent circle diameter of 0.20 μm or more and 0.50 μm or less (per area of ​​40 μm×40 μm) on the surface of the magnetic layer determined as follows is also referred to as "the number of recesses having an equivalent circle diameter in the above range" or simply "the number of recesses". The measurement area is a randomly selected 40 μm square (40 μm × 40 μm) area on the magnetic layer surface. Measurements are performed at three different measurement points on the magnetic layer surface (n = 3). The arithmetic mean of the three measurement results obtained by such measurements is the number of depressions with a circle equivalent diameter of 0.20 μm to 0.50 μm on the surface of the magnetic layer of the magnetic recording medium to be measured. In a planar image of the magnetic layer surface obtained using an AFM, a surface where the volume of the convex component and the concave component in the measurement area are equal is defined as a reference plane, and a part detected as a part that is concave from this reference plane is specified as a "dent". Among the parts specified as dents, there may be some dents that are partly within the measurement area and other parts outside the measurement area. When calculating the number of dents, the number of dents including such dents is counted. In a planar image of the magnetic layer surface obtained using AFM, the area of ​​the portion identified as a recess (hereinafter, "area A") is measured, and the equivalent circle diameter L is calculated by (A / π)^(1 / 2)×2=L. Here, the operator "^" represents exponentiation. The equivalent circle diameter is calculated in units of μm, rounded off to three decimal places and truncated to four decimal places and beyond, in increments of 0.01 μm. The following measurement conditions can be given as an example of the AFM measurement conditions. An AFM (BRUKER Nanoscope 5) is used in peak force tapping mode to measure an area of ​​40 μm × 40 μm on the surface of the magnetic layer of the magnetic recording medium. A BRUKER SCANASYST-AIR probe is used, with a resolution of 512 pixels × 512 pixels and a scan speed of 512 seconds per screen (512 pixels × 512 pixels).

[0034] The number of recesses having a circle equivalent diameter of 0.20 μm or more and 0.50 μm or less present on the surface of the magnetic layer of the magnetic tape is 10 or more and 500 or less per 40 μm×40 μm area. The present inventor speculates that this leads to improved running stability when the magnetic tape is wound around a cartridge reel with a tension of 0.40 N or less. In this regard, the present inventor speculates that the presence of recesses of the above size and number on the surface of the magnetic layer makes it possible to wind the magnetic tape more uniformly when winding with a tension of 0.40 N or less, and / or contributes to stabilizing the contact state between the magnetic tape transport system (e.g., guide, etc.) and the magnetic tape, and as a result, the running stability can be improved when the magnetic tape is wound around a cartridge reel with a tension of 0.40 N or less. However, the present invention is not limited to the speculation described in this specification. From the viewpoint of improving running stability during winding with a tension of 0.40 N or less, the number of dents having a circle-equivalent diameter in the above range is 500 or less, preferably 400 or less, more preferably 300 or less, and even more preferably 200 or less. Also, from the viewpoint of improving running stability during winding with a tension of 0.40 N or less, the number of dents having a circle-equivalent diameter in the above range is 10 or more, preferably 50 or more, and more preferably 100 or more. An example of a method for controlling the number of recesses will be described in detail later.

[0035] <Vertical squareness ratio> In one embodiment, the perpendicular squareness of the magnetic tape can be, for example, 0.55 or more, and is preferably 0.60 or more. It is preferable that the perpendicular squareness of the magnetic tape is 0.60 or more from the viewpoint of improving electromagnetic conversion characteristics. The upper limit of the squareness is, in principle, 1.00 or less. The perpendicular squareness of the magnetic tape can be 1.00 or less, and can be 0.95 or less, 0.90 or less, 0.85 or less, or 0.80 or less. It is preferable that the perpendicular squareness of the magnetic tape has a large value from the viewpoint of improving electromagnetic conversion characteristics. The perpendicular squareness of the magnetic tape can be controlled by a known method such as performing a perpendicular orientation process.

[0036] In the present invention and this specification, the "perpendicular squareness" refers to the squareness measured in the perpendicular direction of the magnetic tape. The "perpendicular direction" described in relation to the squareness is the direction perpendicular to the magnetic layer surface, and can also be called the thickness direction. In the present invention and this specification, the perpendicular squareness is determined by the following method. A sample piece of a size that can be introduced into a vibration sample magnetometer is cut out from the magnetic tape to be measured. A magnetic field is applied to this sample piece in a vertical direction (perpendicular to the magnetic layer surface) using a vibration sample magnetometer at a maximum applied magnetic field of 3979 kA / m, a measurement temperature of 296 K, and a magnetic field sweep speed of 8.3 kA / m / sec, and the magnetization strength of the sample piece against the applied magnetic field is measured. The measured value of the magnetization strength is obtained as a value after demagnetization field correction and a value obtained by subtracting the magnetization of the sample probe of the vibration sample magnetometer as background noise. When the magnetization strength at the maximum applied magnetic field is Ms and the magnetization strength at zero applied magnetic field is Mr, the squareness ratio SQ is a value calculated as SQ=Mr / Ms. The measurement temperature refers to the temperature of the sample piece, and by setting the ambient temperature around the sample piece to the measurement temperature, the temperature equilibrium is established and the temperature of the sample piece can be set to the measurement temperature.

[0037] The above magnetic tape will now be described in more detail.

[0038] <Magnetic layer> (Ferromagnetic powder) As the ferromagnetic powder contained in the magnetic layer, one or more of the ferromagnetic powders known as ferromagnetic powders used in the magnetic layers of various magnetic recording media can be used in combination. It is preferable to use ferromagnetic powders with a small average particle size from the viewpoint of improving recording density. From this viewpoint, the average particle size of the ferromagnetic powder is preferably 50 nm or less, more preferably 45 nm or less, even more preferably 40 nm or less, even more preferably 35 nm or less, even more preferably 30 nm or less, even more preferably 25 nm or less, and even more preferably 20 nm or less. On the other hand, from the viewpoint of magnetization stability, the average particle size of the ferromagnetic powder is preferably 5 nm or more, more preferably 8 nm or more, even more preferably 10 nm or more, even more preferably 15 nm or more, and even more preferably 20 nm or more.

[0039] Hexagonal Ferrite Powder A preferred specific example of the ferromagnetic powder is hexagonal ferrite powder. For details of the hexagonal ferrite powder, see, for example, JP2011-225417A, paragraphs 0012-0030, JP2011-216149A, paragraphs 0134-0136, JP2012-204726A, paragraphs 0013-0030, and JP2015-127985A, paragraphs 0029-0084.

[0040] In the present invention and this specification, the term "hexagonal ferrite powder" refers to a ferromagnetic powder in which a hexagonal ferrite type crystal structure is detected as the main phase by X-ray diffraction analysis. The main phase refers to a structure to which the most intense diffraction peak belongs in the X-ray diffraction spectrum obtained by X-ray diffraction analysis. For example, when the most intense diffraction peak in the X-ray diffraction spectrum obtained by X-ray diffraction analysis is assigned to a hexagonal ferrite type crystal structure, it is determined that the hexagonal ferrite type crystal structure has been detected as the main phase. When only a single structure is detected by X-ray diffraction analysis, the detected structure is regarded as the main phase. The hexagonal ferrite type crystal structure contains at least an iron atom, a divalent metal atom, and an oxygen atom as constituent atoms. The divalent metal atom is a metal atom that can become a divalent cation as an ion, and examples of such include alkaline earth metal atoms such as strontium atoms, barium atoms, and calcium atoms, and lead atoms. In the present invention and this specification, the hexagonal strontium ferrite powder refers to a powder in which the main divalent metal atom contained therein is a strontium atom, and the hexagonal barium ferrite powder refers to a powder in which the main divalent metal atom contained therein is a barium atom. The main divalent metal atom refers to the divalent metal atom that is the most abundant of the divalent metal atoms contained in the powder on an atomic % basis. However, the above divalent metal atoms do not include rare earth atoms. In the present invention and this specification, the "rare earth atom" is selected from the group consisting of scandium atoms (Sc), yttrium atoms (Y), and lanthanoid atoms. The lanthanide atom is selected from the group consisting of a lanthanum atom (La), a cerium atom (Ce), a praseodymium atom (Pr), a neodymium atom (Nd), a promethium atom (Pm), a samarium atom (Sm), a europium atom (Eu), a gadolinium atom (Gd), a terbium atom (Tb), a dysprosium atom (Dy), a holmium atom (Ho), an erbium atom (Er), a thulium atom (Tm), a ytterbium atom (Yb), and a lutetium atom (Lu).

[0041] Hereinafter, hexagonal strontium ferrite powder, which is one form of hexagonal ferrite powder, will be described in more detail.

[0042] The activation volume of the hexagonal strontium ferrite powder is preferably 800 to 1600 nm 3 The finely divided hexagonal strontium ferrite powder having an activation volume in the above range is suitable for producing a magnetic tape exhibiting excellent electromagnetic conversion characteristics. The activation volume of the hexagonal strontium ferrite powder is preferably 800 nm 3 For example, 850 nm or more. 3 From the viewpoint of further improving the electromagnetic conversion characteristics, the activation volume of the hexagonal strontium ferrite powder can be 1500 nm or more. 3 More preferably, it is 1400 nm or less. 3 More preferably, it is 1300 nm or less. 3 More preferably, it is 1200 nm or less. 3 More preferably, it is equal to or less than 1100 nm. 3 It is even more preferable that the activation volume of the hexagonal barium ferrite powder is equal to or less than 1000 nm. The same is true for the activation volume of the hexagonal barium ferrite powder.

[0043] "Activation volume" is a unit of magnetization reversal and is an index showing the magnetic size of a particle. The activation volume and the anisotropy constant Ku described in the present invention and this specification are values ​​obtained by measuring the coercive force Hc measurement section at magnetic field sweep speeds of 3 minutes and 30 minutes (measurement temperature: 23°C ± 1°C) using a vibrating sample magnetometer, and calculating from the following relationship between Hc and activation volume V. The unit of the anisotropy constant Ku is 1 erg / cc = 1.0 x 10 -1 J / m 3 It is. Hc=2Ku / Ms{1-[(kT / KuV)ln(At / 0.693)] 1 / 2} [In the above formula, Ku: anisotropy constant (unit: J / m 3 ), Ms: saturation magnetization (unit: kA / m), k: Boltzmann constant, T: absolute temperature (unit: K), V: activation volume (unit: cm 3), A: spin precession frequency (unit: s -1 ), t: magnetic field reversal time (unit: s)]

[0044] The anisotropy constant Ku can be used as an index of reduction in thermal fluctuation, in other words, improvement in thermal stability. The hexagonal strontium ferrite powder is preferably 1.8×10 5 J / m 3 More preferably, the Ku is 2.0×10 or more. 5 J / m 3 The Ku of the hexagonal strontium ferrite powder can be, for example, 2.5×10 5 J / m 3 However, since a higher Ku value means higher thermal stability and is preferable, the Ku value is not limited to the above-mentioned values.

[0045] The hexagonal strontium ferrite powder may or may not contain rare earth atoms. When the hexagonal strontium ferrite powder contains rare earth atoms, it is preferable that the rare earth atoms are contained at a content (bulk content) of 0.5 to 5.0 atomic % relative to 100 atomic % of iron atoms. In one embodiment, the hexagonal strontium ferrite powder containing rare earth atoms can have uneven distribution of rare earth atoms in the surface layer portion. In the present invention and this specification, the term "surface distribution of rare earth atoms" refers to the rare earth atom content relative to 100 atomic % of iron atoms in a solution obtained by partially dissolving a hexagonal strontium ferrite powder in an acid (hereinafter referred to as "surface content of rare earth atoms" or simply "surface content" for rare earth atoms), which is greater than the rare earth atom content relative to 100 atomic % of iron atoms in a solution obtained by completely dissolving a hexagonal strontium ferrite powder in an acid (hereinafter referred to as "bulk content of rare earth atoms" or simply "bulk content" for rare earth atoms), Rare earth atom surface content / rare earth atom bulk content>1.0 The rare earth atom content of the hexagonal strontium ferrite powder described later is synonymous with the rare earth atom bulk content. In contrast, partial dissolution using an acid dissolves the surface layer of the particles constituting the hexagonal strontium ferrite powder, so the rare earth atom content in the solution obtained by partial dissolution is the rare earth atom content in the surface layer of the particles constituting the hexagonal strontium ferrite powder. The rare earth atom surface layer content satisfying the ratio of "rare earth atom surface layer content / rare earth atom bulk content>1.0" means that the rare earth atoms are unevenly distributed (i.e., more present in the surface layer) in the particles constituting the hexagonal strontium ferrite powder. In the present invention and this specification, the surface layer refers to a portion of the region extending from the surface of the particles constituting the hexagonal strontium ferrite powder toward the inside.

[0046] When the hexagonal strontium ferrite powder contains rare earth atoms, the rare earth atom content (bulk content) is preferably in the range of 0.5 to 5.0 atomic % relative to 100 atomic % of iron atoms. It is considered that the rare earth atoms contained in the bulk content in the above range and the rare earth atoms unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder contribute to suppressing the decrease in the reproduction output during repeated reproduction. This is presumed to be because the hexagonal strontium ferrite powder contains rare earth atoms in the bulk content in the above range and the rare earth atoms unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder can increase the anisotropy constant Ku. The higher the value of the anisotropy constant Ku, the more the occurrence of a phenomenon called thermal fluctuation can be suppressed (in other words, the thermal stability can be improved). By suppressing the occurrence of thermal fluctuation, the decrease in the reproduction output during repeated reproduction can be suppressed. It is speculated that the uneven distribution of rare earth atoms in the surface layer of hexagonal strontium ferrite powder particles contributes to stabilizing the spin of the iron (Fe) sites in the crystal lattice of the surface layer, thereby increasing the anisotropy constant Ku. In addition, it is presumed that using the hexagonal strontium ferrite powder having rare earth atom uneven distribution on the surface as the ferromagnetic powder of the magnetic layer also contributes to suppressing the wear of the magnetic layer surface due to sliding with the magnetic head. That is, it is presumed that the hexagonal strontium ferrite powder having rare earth atom uneven distribution on the surface can also contribute to improving the running durability of the magnetic tape. This is presumed to be because the uneven distribution of rare earth atoms on the surface of the particles constituting the hexagonal strontium ferrite powder contributes to improving the interaction between the particle surface and the organic substance (e.g., binder and / or additive) contained in the magnetic layer, and as a result, the strength of the magnetic layer is improved. From the viewpoint of further suppressing the decrease in regeneration output during repeated regeneration and / or further improving running durability, the rare earth atom content (bulk content) is more preferably in the range of 0.5 to 4.5 atomic %, even more preferably in the range of 1.0 to 4.5 atomic %, and even more preferably in the range of 1.5 to 4.5 atomic %.

[0047] The bulk content is the content obtained by completely dissolving the hexagonal strontium ferrite powder. In the present invention and this specification, unless otherwise specified, the content of an atom refers to the bulk content obtained by completely dissolving the hexagonal strontium ferrite powder. The hexagonal strontium ferrite powder containing rare earth atoms may contain only one rare earth atom as a rare earth atom, or may contain two or more rare earth atoms. When two or more rare earth atoms are contained, the bulk content is obtained for the total of two or more rare earth atoms. This point is the same for other components in the present invention and this specification. That is, unless otherwise specified, a certain component may be used in only one type, or in two or more types. When two or more types are used, the content or content refers to the total of two or more types.

[0048] When the hexagonal strontium ferrite powder contains rare earth atoms, the rare earth atoms contained therein may be any one or more of rare earth atoms. From the viewpoint of further suppressing the decrease in the reproduction output during repeated reproduction, preferred rare earth atoms include neodymium atoms, samarium atoms, yttrium atoms and dysprosium atoms, more preferred are neodymium atoms, samarium atoms and yttrium atoms, and even more preferred are neodymium atoms.

[0049] In the hexagonal strontium ferrite powder having rare earth atom uneven distribution in the surface layer, the rare earth atoms may be unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder, and the degree of uneven distribution is not limited. For example, for the hexagonal strontium ferrite powder having rare earth atom uneven distribution in the surface layer, the ratio of the surface content of rare earth atoms obtained by partial dissolution under the dissolution conditions described below to the bulk content of rare earth atoms obtained by complete dissolution under the dissolution conditions described below, "surface content / bulk content", is more than 1.0 and can be 1.5 or more. The "surface content / bulk content" being greater than 1.0 means that the rare earth atoms are unevenly distributed in the surface layer (i.e., more than in the interior) in the particles constituting the hexagonal strontium ferrite powder. In addition, the ratio of the surface layer content of rare earth atoms obtained by partial dissolution under the dissolution conditions described later to the bulk content of rare earth atoms obtained by total dissolution under the dissolution conditions described later, "surface layer content / bulk content", can be, for example, 10.0 or less, 9.0 or less, 8.0 or less, 7.0 or less, 6.0 or less, 5.0 or less, or 4.0 or less. However, in a hexagonal strontium ferrite powder having rare earth atom surface layer uneven distribution, it is sufficient that the rare earth atoms are unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder, and the above "surface layer content / bulk content" is not limited to the upper or lower limit exemplified.

[0050] The partial and total dissolution of hexagonal strontium ferrite powder will be described below. For hexagonal strontium ferrite powder present as powder, the sample powders to be partially and completely dissolved are taken from the same lot of powder. On the other hand, for hexagonal strontium ferrite powder contained in the magnetic layer of a magnetic tape, a part of the hexagonal strontium ferrite powder taken out from the magnetic layer is subjected to partial dissolution, and the other part is subjected to total dissolution. The hexagonal strontium ferrite powder can be taken out from the magnetic layer by, for example, the method described in paragraph 0032 of JP 2015-91747 A. The above-mentioned partial dissolution means that the hexagonal strontium ferrite powder is dissolved to such an extent that the remaining powder can be visually confirmed in the liquid at the end of dissolution. For example, the partial dissolution can dissolve a region of 10 to 20 mass% of the particles constituting the hexagonal strontium ferrite powder, with the whole particles being 100 mass%. On the other hand, the above-mentioned complete dissolution means that the hexagonal strontium ferrite powder is dissolved to such an extent that the remaining powder cannot be visually confirmed in the liquid at the end of dissolution. The partial dissolution and the surface layer content are measured, for example, by the following method. Note that the dissolution conditions such as the amount of sample powder are merely examples, and any dissolution conditions that allow partial or complete dissolution can be used. A container (e.g., a beaker) containing 12 mg of sample powder and 10 mL of 1 mol / L hydrochloric acid is placed on a hot plate set at 70°C for 1 hour. The resulting solution is filtered through a 0.1 μm membrane filter. Elemental analysis of the filtrate thus obtained is performed using an inductively coupled plasma (ICP) analyzer. In this way, the surface layer content of rare earth atoms relative to 100 atomic % of iron atoms can be determined. When multiple types of rare earth atoms are detected by elemental analysis, the total content of all rare earth atoms is taken as the surface layer content. This is also true for the measurement of bulk content. On the other hand, the total dissolved and bulk contents are measured, for example, by the following method. A container (e.g., a beaker) containing 12 mg of sample powder and 10 mL of 4 mol / L hydrochloric acid is placed on a hot plate set at 80° C. for 3 hours. After that, the bulk content relative to 100 atomic % of iron atoms can be calculated by carrying out the same procedure as the partial dissolution and surface layer content measurement described above.

[0051] From the viewpoint of increasing the reproduction output when reproducing data recorded on a magnetic tape, it is desirable for the mass magnetization σs of the ferromagnetic powder contained in the magnetic tape to be high. In this regard, hexagonal strontium ferrite powder that contains rare earth atoms but does not have uneven distribution of rare earth atoms in the surface layer has a tendency to have a significantly lower σs than hexagonal strontium ferrite powder that does not contain rare earth atoms. In contrast, hexagonal strontium ferrite powder that has uneven distribution of rare earth atoms in the surface layer is considered to be preferable in terms of suppressing such a large decrease in σs. In one embodiment, the σs of the hexagonal strontium ferrite powder is 45 A·m 2 / kg or more, and 47A·m 2 / kg or more. On the other hand, from the viewpoint of noise reduction, σs is 80A·m 2 / kg or less, and 60A·m 2 / kg or less. σs can be measured using a known measuring device capable of measuring magnetic properties, such as a vibrating sample magnetometer. In the present invention and this specification, unless otherwise specified, the mass magnetization σs is a value measured at a magnetic field strength of 15 kOe. 1 [kOe]=10 6 / 4π[A / m].

[0052] Regarding the content (bulk content) of the constituent atoms of the hexagonal strontium ferrite powder, the strontium atom content can be, for example, in the range of 2.0 to 15.0 atomic % relative to 100 atomic % of iron atoms. In one embodiment, the divalent metal atoms contained in the hexagonal strontium ferrite powder can be only strontium atoms. In another embodiment, the hexagonal strontium ferrite powder can also contain one or more other divalent metal atoms in addition to strontium atoms. For example, it can contain barium atoms and / or calcium atoms. When divalent metal atoms other than strontium atoms are contained, the barium atom content and calcium atom content in the hexagonal strontium ferrite powder can each be, for example, in the range of 0.05 to 5.0 atomic % relative to 100 atomic % of iron atoms.

[0053] Known crystal structures of hexagonal ferrite include magnetoplumbite type (also called "M type"), W type, Y type, and Z type. The hexagonal strontium ferrite powder may have any of the crystal structures. The crystal structure can be confirmed by X-ray diffraction analysis. The hexagonal strontium ferrite powder may be one in which a single crystal structure or two or more types of crystal structures are detected by X-ray diffraction analysis. For example, in one embodiment, the hexagonal strontium ferrite powder may be one in which only the M-type crystal structure is detected by X-ray diffraction analysis. For example, M-type hexagonal ferrite is AFe 12 O 19Here, A represents a divalent metal atom, and when the hexagonal strontium ferrite powder is of the M type, A is only a strontium atom (Sr), or when A contains a plurality of divalent metal atoms, the strontium atom (Sr) accounts for the largest proportion on an atomic % basis as described above. The divalent metal atom content of the hexagonal strontium ferrite powder is usually determined by the type of crystal structure of the hexagonal ferrite, and is not particularly limited. The same applies to the iron atom content and the oxygen atom content. The hexagonal strontium ferrite powder contains at least an iron atom, a strontium atom, and an oxygen atom, and may further contain a rare earth atom. Furthermore, the hexagonal strontium ferrite powder may or may not contain atoms other than these atoms. As an example, the hexagonal strontium ferrite powder may contain an aluminum atom (Al). The content of aluminum atoms can be, for example, 0.5 to 10.0 atomic % relative to 100 atomic % of iron atoms. From the viewpoint of further suppressing the decrease in the reproduction output during repeated reproduction, the hexagonal strontium ferrite powder contains iron atoms, strontium atoms, oxygen atoms, and rare earth atoms, and the content of atoms other than these atoms is preferably 10.0 atomic % or less, more preferably in the range of 0 to 5.0 atomic %, relative to 100 atomic % of iron atoms, and may be 0 atomic %. That is, in one embodiment, the hexagonal strontium ferrite powder may not contain atoms other than iron atoms, strontium atoms, oxygen atoms, and rare earth atoms. The content expressed in atomic % above is obtained by converting the content (unit: mass %) of each atom obtained by completely dissolving the hexagonal strontium ferrite powder into a value expressed in atomic % using the atomic weight of each atom. In addition, in the present invention and this specification, "not containing" a certain atom means that the content measured by an ICP analyzer after completely dissolving is 0 mass %. The detection limit of an ICP analyzer is usually 0.01 ppm (parts per million) or less on a mass basis. The above term "free" is used to mean that the content is below the detection limit of the ICP analyzer.In one form, the hexagonal strontium ferrite powder can be one that does not contain bismuth atoms (Bi).

[0054] metal powder A specific preferred example of the ferromagnetic powder is a ferromagnetic metal powder. For details of the ferromagnetic metal powder, reference can be made to, for example, paragraphs 0137 to 0141 of JP 2011-216149 A and paragraphs 0009 to 0023 of JP 2005-251351 A.

[0055] ε-iron oxide powder A preferred specific example of the ferromagnetic powder is ε-iron oxide powder. In the present invention and this specification, the term "ε-iron oxide powder" refers to a ferromagnetic powder in which an ε-iron oxide type crystal structure is detected as the main phase by X-ray diffraction analysis. For example, when the highest intensity diffraction peak in the X-ray diffraction spectrum obtained by X-ray diffraction analysis is attributed to an ε-iron oxide type crystal structure, it is determined that the ε-iron oxide type crystal structure is detected as the main phase. Known methods for producing ε-iron oxide powder include a method of producing it from goethite and a reverse micelle method. All of the above production methods are publicly known. In addition, for a method for producing ε-iron oxide powder in which a part of Fe is replaced by a substitution atom such as Ga, Co, Ti, Al, or Rh, reference can be made to, for example, J. Jpn. Soc. Powder Metallurgy Vol. 61 Supplement, No. S1, pp. S280-S284, J. Mater. Chem. C, 2013, 1, pp.5200-5206, etc. However, the method for producing the ε-iron oxide powder that can be used as the ferromagnetic powder in the magnetic layer of the magnetic tape is not limited to the method given here.

[0056] The activation volume of the ε-iron oxide powder is preferably 300 to 1500 nm 3 The finely divided ε-iron oxide powder exhibiting an activation volume in the above range is suitable for producing a magnetic tape exhibiting excellent electromagnetic conversion characteristics. The activation volume of the ε-iron oxide powder is preferably 300 nm 3For example, 500 nm or more. 3 From the viewpoint of further improving the electromagnetic conversion characteristics, the activation volume of the ε-iron oxide powder can be 1400 nm or more. 3 More preferably, it is 1300 nm or less. 3 More preferably, it is 1200 nm or less. 3 More preferably, it is equal to or less than 1100 nm. 3 It is even more preferred that:

[0057] The anisotropy constant Ku can be used as an index of the reduction in thermal fluctuation, in other words, the improvement in thermal stability. The ε-iron oxide powder is preferably 3.0×10 4 J / m 3 More preferably, the Ku is 8.0×10 or more. 4 J / m 3 The Ku of the ε-iron oxide powder can be, for example, 3.0×10 5 J / m 3 However, since a higher Ku value means higher thermal stability and is preferable, the Ku value is not limited to the above-mentioned values.

[0058] From the viewpoint of increasing the reproduction output when reproducing data recorded on a magnetic tape, it is desirable that the mass magnetization σs of the ferromagnetic powder contained in the magnetic tape is high. In this regard, in one embodiment, the σs of the ε-iron oxide powder is 8 A m 2 / kg or more, and 12 A m 2 On the other hand, the σs of ε-iron oxide powder is 40 A m 2 / kg or less, and 35A·m 2 It is more preferable that the amount is not more than 1 / kg.

[0059] In the present invention and this specification, unless otherwise specified, the average particle size of various powders such as ferromagnetic powders is a value measured by the following method using a transmission electron microscope. The powder is photographed at a magnification of 100,000 times using a transmission electron microscope, and then printed on photographic paper at a total magnification of 500,000 times to obtain a photograph of the particles that make up the powder. From the obtained particle photograph, the target particle is selected, the particle's outline is traced with a digitizer, and the particle (primary particle) size is measured. Primary particles are independent particles that are not aggregated. The above measurements are carried out for 500 randomly selected particles. The arithmetic mean of the particle sizes of the 500 particles thus obtained is the average particle size of the powder. As the transmission electron microscope, for example, a Hitachi transmission electron microscope H-9000 type can be used. The particle size can be measured using known image analysis software, for example, Carl Zeiss image analysis software KS-400. The average particle size shown in the examples described below is a value measured using a Hitachi transmission electron microscope H-9000 type as the transmission electron microscope and Carl Zeiss image analysis software KS-400 as the image analysis software, unless otherwise specified. In the present invention and this specification, powder means a collection of multiple particles. For example, ferromagnetic powder means a collection of multiple ferromagnetic particles. In addition, the collection of multiple particles is not limited to a form in which the particles constituting the collection are in direct contact with each other, and also includes a form in which a binder, additive, etc., described later, are interposed between the particles. The term particle is sometimes used to refer to powder.

[0060] As a method for collecting sample powder from the magnetic tape for particle size measurement, for example, the method described in paragraph 0015 of JP 2011-048878 A can be used.

[0061] In the present invention and this specification, unless otherwise specified, the size of the particles constituting the powder (particle size) is determined by the shape of the particles observed in the particle photograph. (1) In the case of needle-shaped, spindle-shaped, columnar (where the height is greater than the maximum major axis of the base), etc., it is expressed by the length of the major axis that constitutes the particle, i.e., the major axis length. (2) In the case of a plate or columnar shape (where the thickness or height is smaller than the maximum long diameter of the plate or base), it shall be expressed by the maximum long diameter of the plate or base. (3) In the case of a particle having a spherical, polyhedral, or amorphous shape, and in which the major axis of the particle cannot be identified from its shape, the particle is expressed as the equivalent circle diameter, which is determined by the circle projection method.

[0062] The average acicular ratio of a powder refers to the arithmetic average of the short axis length of the particles, i.e., the short axis length, the (long axis length / short axis length) value of each particle, and the values ​​obtained for the 500 particles. Here, unless otherwise specified, the short axis length refers to the length of the short axis constituting the particle in the above definition of particle size (1), and to the thickness or height in the above definition of particle size (2), and in the above definition of particle size (3), since there is no distinction between the long axis and the short axis, (long axis length / short axis length) is considered to be 1 for the sake of convenience. Unless otherwise specified, when the particle shape is specific, for example, in the case of the above definition of particle size (1), the average particle size is the average major axis length, in the case of definition (2), the average particle size is the average plate diameter, and in the case of definition (3), the average particle size is the average diameter (also called the average particle diameter or average particle size).

[0063] The content (filling rate) of the ferromagnetic powder in the magnetic layer is preferably in the range of 50 to 90 mass % and more preferably in the range of 60 to 90 mass % relative to the total mass of the magnetic layer. A high filling rate of the ferromagnetic powder in the magnetic layer is preferable from the viewpoint of improving recording density.

[0064] (Binding Agent) The magnetic tape may be a coated magnetic tape, and may contain a binder in the magnetic layer. The binder is one or more kinds of resin. As the binder, various resins that are usually used as binders for coated magnetic tapes may be used. For example, as the binder, a resin selected from polyurethane resin, polyester resin, polyamide resin, vinyl chloride resin, acrylic resin copolymerized with styrene, acrylonitrile, methyl methacrylate, etc., cellulose resin such as nitrocellulose, epoxy resin, phenoxy resin, polyvinyl acetal, polyvinyl butyral, etc. may be used alone or in combination of a plurality of resins. Among these, polyurethane resin, acrylic resin, cellulose resin, and vinyl chloride resin are preferred. These resins may be homopolymers or copolymers. These resins may also be used as binders in the non-magnetic layer and / or backcoat layer described below. For the above binders, reference can be made to paragraphs 0028 to 0031 of JP 2010-24113 A. The average molecular weight of the resin used as the binder can be, for example, 10,000 to 200,000 in weight average molecular weight. The binder can be used in an amount of, for example, 1.0 to 30.0 parts by mass relative to 100.0 parts by mass of the ferromagnetic powder.

[0065] (hardening agent) A curing agent can be used together with the resin usable as a binder. In one embodiment, the curing agent can be a thermosetting compound, which is a compound in which a curing reaction (crosslinking reaction) proceeds by heating, and in another embodiment, the curing agent can be a photocuring compound in which a curing reaction (crosslinking reaction) proceeds by light irradiation. As the curing reaction proceeds in the magnetic layer forming process, at least a part of the curing agent can be contained in the magnetic layer in a state of reacting (crosslinking) with other components such as the binder. This point is also true for layers formed using a composition used to form other layers that contains a curing agent. A preferred curing agent is a thermosetting compound, and polyisocyanate is suitable. For details on polyisocyanate, refer to paragraphs 0124 to 0125 of JP 2011-216149 A. The curing agent can be used in an amount of, for example, 0 to 80.0 parts by mass relative to 100.0 parts by mass of the binder, and preferably 50.0 to 80.0 parts by mass from the viewpoint of improving the strength of the magnetic layer.

[0066] (Additives) The magnetic layer may contain one or more additives as necessary. The additives may be selected from commercially available products according to the desired properties. Alternatively, compounds synthesized by known methods may be used as additives. The additives may be used in any amount. An example of the additive is the above-mentioned curing agent. Examples of additives contained in the magnetic layer include non-magnetic powders (e.g., inorganic powders, carbon black, etc.), lubricants, dispersants, dispersion aids, antifungal agents, antistatic agents, antioxidants, etc. For example, reference may be made to paragraphs 0030 to 0033, 0035, and 0036 of JP-A-2016-126817 for lubricants. The non-magnetic layer described below may contain a lubricant. Reference may be made to paragraphs 0030 to 0031, 0034, 0035, and 0036 of JP-A-2016-126817 for lubricants that may be contained in the non-magnetic layer. For the dispersant, refer to paragraphs 0061 and 0071 of JP-A-2012-133837. The dispersant may be added to the non-magnetic layer forming composition. For the dispersant that can be added to the non-magnetic layer forming composition, refer to paragraph 0061 of JP-A-2012-133837. In addition, examples of non-magnetic powders that can be included in the magnetic layer include non-magnetic powders that can function as abrasives, and non-magnetic powders (e.g., non-magnetic colloidal particles) that can function as protrusion-forming agents that form protrusions that protrude appropriately on the magnetic layer surface. For example, for the abrasives, refer to paragraphs 0030 to 0032 of JP-A-2004-273070. As the protrusion-forming agent, colloidal particles are preferred, and inorganic colloidal particles are preferred from the viewpoint of availability, inorganic oxide colloidal particles are more preferred, and silica colloidal particles (colloidal silica) are even more preferred. The average particle size of each of the abrasive and protrusion-forming agent is preferably in the range of 30 to 200 nm, and more preferably in the range of 50 to 100 nm.

[0067] The magnetic layer described above can be provided directly on the surface of the non-magnetic support, or indirectly via a non-magnetic layer.

[0068] <Nonmagnetic layer> Next, the non-magnetic layer will be described. The magnetic tape may have a magnetic layer directly on the surface of the non-magnetic support, or may have a magnetic layer on the surface of the non-magnetic support via a non-magnetic layer containing non-magnetic powder. The non-magnetic powder used in the non-magnetic layer may be an inorganic powder or an organic powder. Carbon black or the like may also be used. Examples of inorganic powder include powders of metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, metal sulfides, and the like. These non-magnetic powders are commercially available, and can also be produced by known methods. For details, refer to paragraphs 0146 to 0150 of JP-A-2011-216149. For carbon black usable in the non-magnetic layer, refer to paragraphs 0040 and 0041 of JP-A-2010-24113. The content (filling rate) of the non-magnetic powder in the non-magnetic layer is preferably in the range of 50 to 90% by mass, more preferably in the range of 60 to 90% by mass, based on the total mass of the non-magnetic layer.

[0069] The non-magnetic layer may contain a binder and may also contain an additive. For other details of the binder, additive, etc. of the non-magnetic layer, known techniques related to non-magnetic layers can be applied. In addition, for example, for the type and content of the binder, the type and content of the additive, known techniques related to magnetic layers can also be applied.

[0070] In the present invention and this specification, the nonmagnetic layer also includes a substantially nonmagnetic layer that contains a small amount of ferromagnetic powder, for example as an impurity or intentionally, together with the nonmagnetic powder. Here, the substantially nonmagnetic layer refers to a layer having a residual magnetic flux density of 10 mT or less, a coercive force of 7.96 kA / m (100 Oe) or less, or a layer having a residual magnetic flux density of 10 mT or less and a coercive force of 7.96 kA / m (100 Oe) or less. It is preferable that the nonmagnetic layer has no residual magnetic flux density or coercive force.

[0071] <Nonmagnetic support> Examples of the non-magnetic support (hereinafter also simply referred to as "support") include known biaxially stretched polyethylene terephthalate, polyethylene naphthalate, polyamide, polyamideimide, aromatic polyamide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred.

[0072] In one embodiment, the non-magnetic support of the magnetic tape may be an aromatic polyester support. In the present invention and this specification, "aromatic polyester" means a resin containing an aromatic skeleton and a plurality of ester bonds, and "aromatic polyester support" means a support containing at least one layer of aromatic polyester film. "Aromatic polyester film" means a film in which the component that constitutes this film in the largest proportion by mass is an aromatic polyester. In the present invention and this specification, the "aromatic polyester support" includes a support in which all the resin films contained in this support are aromatic polyester films, and a support containing an aromatic polyester film and another resin film. Specific embodiments of the aromatic polyester support include a single-layer aromatic polyester film, a laminated film of two or more layers of aromatic polyester films having the same constituent components, a laminated film of two or more layers of aromatic polyester films having different constituent components, a laminated film containing one or more layers of aromatic polyester films and one or more layers of resin films other than aromatic polyesters, and the like. In the laminated film, an adhesive layer or the like may be optionally included between two adjacent layers. In addition, the aromatic polyester support may optionally include a metal film and / or a metal oxide film formed by deposition or the like on one or both surfaces. The above also applies to the "polyethylene terephthalate support" and the "polyethylene naphthalate support" in the present invention and this specification.

[0073] The aromatic ring contained in the aromatic skeleton of the aromatic polyester is not particularly limited, and specific examples of the aromatic ring include a benzene ring and a naphthalene ring. For example, polyethylene terephthalate (PET) is a polyester containing a benzene ring, and is a resin obtained by polycondensation of ethylene glycol with terephthalic acid and / or dimethyl terephthalate. In the present invention and this specification, "polyethylene terephthalate" also includes structures having one or more other components (e.g., copolymerized components, components introduced into the terminals or side chains, etc.) in addition to the above components. Polyethylene naphthalate (PEN) is a polyester containing a naphthalene ring, and is a resin obtained by esterification of dimethyl 2,6-naphthalenedicarboxylate with ethylene glycol, followed by transesterification and polycondensation. In the present invention and this specification, "polyethylene naphthalate" also includes structures having one or more other components (e.g., copolymer components, components introduced into the terminals or side chains, etc.) in addition to the above components.

[0074] The non-magnetic support may be a biaxially stretched film, and may be a film that has been subjected to corona discharge, plasma treatment, easy-adhesion treatment, heat treatment, or the like.

[0075] <Backcoat layer> The magnetic tape may or may not have a backcoat layer containing a nonmagnetic powder on the surface side of the nonmagnetic support opposite to the surface side having the magnetic layer. For the nonmagnetic powder in the backcoat layer, see the above description of the nonmagnetic powder in the nonmagnetic layer.

[0076] The recesses on the magnetic layer surface can be formed by transferring the surface shape of the back surface to the magnetic layer surface (so-called "show-through") in a state where the magnetic layer surface and the back surface are in contact with each other in a rolled state during the manufacturing process of the magnetic tape. The back surface is the back coat layer surface when the magnetic tape has a back coat layer, and is the support surface when the magnetic tape does not have a back coat layer. One example of a method for controlling the state of the recesses on the magnetic layer surface is, for example, selecting the type of component to be added to the composition for forming the back coat layer in order to adjust the surface shape of the back surface. From this point of view, it is preferable to use carbon black and a non-magnetic powder other than carbon black in combination as the non-magnetic powder of the back coat layer, or to use carbon black (i.e., the non-magnetic powder of the back coat layer is made of carbon black). Examples of non-magnetic powder other than carbon black include the non-magnetic powders exemplified above as those that can be contained in the non-magnetic layer. For the non-magnetic powder in the backcoat layer, the proportion of carbon black in 100.0 parts by mass of the total amount of non-magnetic powder is preferably in the range of 50.0 to 100.0 parts by mass, more preferably in the range of 70.0 to 100.0 parts by mass, and even more preferably in the range of 90.0 to 100.0 parts by mass. It is also preferable that the total amount of non-magnetic powder in the backcoat layer is carbon black. The content (filling rate) of non-magnetic powder in the backcoat layer is preferably in the range of 50 to 90% by mass, more preferably in the range of 60 to 90% by mass, relative to the total mass of the backcoat layer.

[0077] From the viewpoint of ease of control of the number of recesses having a circle equivalent diameter in the above range present on the magnetic layer surface, in one embodiment, it is preferable to use a nonmagnetic powder having an average particle size of 50 nm or less as the nonmagnetic powder of the backcoat layer. As the nonmagnetic powder of the backcoat layer, only one type of nonmagnetic powder may be used, or two or more types can be used. When two or more types (for example, carbon black and a nonmagnetic powder other than carbon black) are used, it is preferable that the average particle size of each is 50 nm or less. The average particle size of the nonmagnetic powder is more preferably in the range of 10 to 50 nm, and even more preferably in the range of 10 to 30 nm. In one embodiment, it is preferable that the entire amount of the nonmagnetic powder contained in the backcoat layer is carbon black, and its average particle size is 50 nm or less.

[0078] In order to control the state of the depressions on the magnetic layer surface, the composition for forming the backcoat layer preferably contains a component (dispersant) capable of increasing the dispersibility of the nonmagnetic powder contained in the composition. The composition for forming the backcoat layer more preferably contains a nonmagnetic powder having an average particle size of 50 nm or less and a component capable of increasing the dispersibility of the nonmagnetic powder, and further preferably contains carbon black having an average particle size of 50 nm or less and a component capable of increasing the dispersibility of the carbon black.

[0079] As an example of such a dispersant, a compound having an ammonium salt structure of an alkyl ester anion represented by the following formula 1 can be used. Note that the "alkyl ester anion" can also be called an "alkyl carboxylate anion."

[0080] [ka]

[0081] In formula 1, R represents an alkyl group having 7 or more carbon atoms or a fluorinated alkyl group having 7 or more carbon atoms; Z + represents an ammonium cation.

[0082] In addition, from the viewpoint of improving the dispersibility of carbon black, in one embodiment, two or more components capable of forming a compound having the above-mentioned salt structure can be used when preparing the composition for forming a backcoat layer, whereby at least a part of the components can form a compound having the above-mentioned salt structure when preparing the composition for forming a backcoat layer.

[0083] Unless otherwise specified, the groups described below may have a substituent or may be unsubstituted. In addition, the "carbon number" of a group having a substituent means the carbon number not including the carbon number of the substituent, unless otherwise specified. In the present invention and this specification, examples of the substituent include an alkyl group (e.g., an alkyl group having 1 to 6 carbon atoms), a hydroxyl group, an alkoxy group (e.g., an alkoxy group having 1 to 6 carbon atoms), a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, etc.), a cyano group, an amino group, a nitro group, an acyl group, a carboxy group, a salt of a carboxy group, a sulfonic acid group, a salt of a sulfonic acid group, etc.

[0084] Formula 1 will now be described in more detail.

[0085] In formula 1, R represents an alkyl group having 7 or more carbon atoms or a fluorinated alkyl group having 7 or more carbon atoms. The fluorinated alkyl group has a structure in which some or all of the hydrogen atoms constituting the alkyl group are substituted with fluorine atoms. The alkyl group or fluorinated alkyl group represented by R may have a straight-chain structure, may have a branched structure, or may be a cyclic alkyl group or fluorinated alkyl group, and is preferably a straight-chain structure. The alkyl group or fluorinated alkyl group represented by R may have a substituent or may be unsubstituted, and is preferably unsubstituted. The alkyl group represented by R is, for example, C n H 2n+1 Here, n is an integer of 7 or more. The fluorinated alkyl group represented by R can be, for example, C n H 2n+1The alkyl group or fluorinated alkyl group represented by R may have a structure in which some or all of the hydrogen atoms constituting the alkyl group represented by - are substituted with fluorine atoms. The number of carbon atoms in the alkyl group or fluorinated alkyl group represented by R is 7 or more, preferably 8 or more, more preferably 9 or more, even more preferably 10 or more, still more preferably 11 or more, even more preferably 12 or more, and even more preferably 13 or more. The number of carbon atoms in the alkyl group or fluorinated alkyl group represented by R is preferably 20 or less, more preferably 19 or less, and even more preferably 18 or less.

[0086] In equation 1, Z + represents an ammonium cation. More specifically, the ammonium cation has the following structure: In the present invention and this specification, "*" in a formula representing a part of a compound represents the bonding position between the part of the structure and the adjacent atom.

[0087] [ka]

[0088] Nitrogen cation N of ammonium cation + and the oxygen anion O in Eq. - and form a salt bridging group to form an ammonium salt structure of an alkyl ester anion represented by formula 1. The inclusion of a compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 in the backcoat layer can be confirmed by analyzing the magnetic tape using X-ray photoelectron spectroscopy (ESCA; Electron Spectroscopy for Chemical Analysis), infrared spectroscopy (IR; infrared spectroscopy), etc.

[0089] In one form, Z +The ammonium cation represented by the formula (I) can be obtained, for example, by the nitrogen atom of a nitrogen-containing polymer becoming a cation. The nitrogen-containing polymer means a polymer containing a nitrogen atom. In the present invention and this specification, the terms "polymer" and "polymeric polymer" are used to include homopolymers and copolymers. In one form, the nitrogen atom can be included as an atom constituting the main chain of the polymer, and in another form, the nitrogen atom can be included as an atom constituting the side chain of the polymer.

[0090] One example of the nitrogen-containing polymer is polyalkyleneimine, which is a ring-opening polymer of alkyleneimine and has a plurality of repeating units represented by the following formula 2.

[0091] [ka]

[0092] The nitrogen atom N constituting the main chain in formula 2 is a nitrogen cation N + So, Z in Eq. + This can result in an ammonium cation represented by the formula: and can form an ammonium salt structure with an alkyl ester anion, for example as follows:

[0093] [ka]

[0094] Formula 2 will now be described in more detail.

[0095] In formula 2, R 1 and R 2 each independently represents a hydrogen atom or an alkyl group, and n1 represents an integer of 2 or greater.

[0096] R 1 or R 2Examples of the alkyl group represented by the formula (I) include alkyl groups having 1 to 6 carbon atoms, preferably alkyl groups having 1 to 3 carbon atoms, more preferably a methyl group or an ethyl group, and even more preferably a methyl group. 1 or R 2 The alkyl group represented by the formula (2) is preferably an unsubstituted alkyl group. 1 and R 2 The combination of includes a form in which one is a hydrogen atom and the other is an alkyl group, a form in which both are hydrogen atoms, and a form in which both are alkyl groups (same or different alkyl groups), and preferably a form in which both are hydrogen atoms. As an alkyleneimine that results in a polyalkyleneimine, the structure with the smallest number of carbon atoms constituting the ring is ethyleneimine, and the number of carbon atoms in the main chain of the alkyleneimine (ethyleneimine) obtained by ring-opening of ethyleneimine is 2. Therefore, n1 in formula 2 is 2 or more. n1 in formula 2 can be, for example, 10 or less, 8 or less, 6 or less, or 4 or less. The polyalkyleneimine may be a homopolymer containing only the same structure as the repeating structure represented by formula 2, or a copolymer containing two or more different structures as the repeating structure represented by formula 2. The number average molecular weight of the polyalkyleneimine that can be used to form a compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 can be, for example, 200 or more, preferably 300 or more, and more preferably 400 or more. The number average molecular weight of the polyalkyleneimine can be, for example, 10,000 or less, preferably 5,000 or less, and more preferably 2,000 or less.

[0097] In the present invention and this specification, the average molecular weight (weight average molecular weight and number average molecular weight) refers to a value measured by gel permeation chromatography (GPC) and calculated in terms of standard polystyrene. The average molecular weight shown in the examples described later is a value (polystyrene-equivalent value) calculated in terms of standard polystyrene from a value measured by GPC under the following measurement conditions, unless otherwise specified. GPC equipment: HLC-8220 (Tosoh Corporation) Guard column: TSKguardcolumn Super HZM-H Columns: TSKgel Super HZ 2000, TSKgel Super HZ 4000, TSKgel Super HZ-M (Tosoh Corporation, 4.6 mm (inner diameter) x 15.0 cm, three columns connected in series) Eluent: Tetrahydrofuran (THF), containing stabilizer (2,6-di-t-butyl-4-methylphenol) Eluent flow rate: 0.35mL / min Column temperature: 40℃ Inlet temperature: 40℃ Refractive Index (RI) measurement temperature: 40℃ Sample concentration: 0.3% by mass Sample injection volume: 10 μL

[0098] Another example of the nitrogen-containing polymer is polyallylamine, which is a polymer of allylamine and has a plurality of repeating units represented by the following formula 3.

[0099] [ka]

[0100] The nitrogen atom N constituting the amino group in the side chain in formula 3 is a nitrogen cation N + So, Z in Eq. + This can result in an ammonium cation represented by the formula: and can form an ammonium salt structure with an alkyl ester anion, for example as follows:

[0101] [ka]

[0102] The weight-average molecular weight of the polyallylamine usable for forming the compound having an ammonium salt structure of the alkyl ester anion represented by formula 1 can be, for example, 200 or more, preferably 1,000 or more, and more preferably 1,500 or more. The weight-average molecular weight of the polyalkyleneimine can be, for example, 15,000 or less, preferably 10,000 or less, and more preferably 8,000 or less.

[0103] The fact that the backcoat layer contains a compound having a structure derived from polyalkyleneimine or polyallylimine as a compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 can be confirmed by analyzing the surface of the backcoat layer using time-of-flight secondary ion mass spectrometry (TOF-SIMS) or the like.

[0104] The compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 can be a salt of a nitrogen-containing polymer and one or more fatty acids selected from the group consisting of fatty acids having 7 or more carbon atoms and fluorinated fatty acids having 7 or more carbon atoms. The nitrogen-containing polymer forming the salt can be one or more nitrogen-containing polymers, for example, a nitrogen-containing polymer selected from the group consisting of polyalkyleneimine and polyallylamine. The fatty acids forming the salt can be one or more fatty acids selected from the group consisting of fatty acids having 7 or more carbon atoms and fluorinated fatty acids having 7 or more carbon atoms. The fluorinated fatty acid has a structure in which some or all of the hydrogen atoms constituting the alkyl group bonded to the carboxy group COOH in the fatty acid are replaced with fluorine atoms. For example, the salt-forming reaction can easily proceed by mixing the nitrogen-containing polymer and the above-mentioned fatty acids at room temperature. The room temperature is, for example, about 20 to 25°C. In one embodiment, one or more nitrogen-containing polymers and one or more fatty acids are used as components of the composition for forming a backcoat layer, and the salt-forming reaction can be promoted by mixing them in the preparation process of the composition for forming a backcoat layer. In another embodiment, before preparing the composition for forming a backcoat layer, one or more nitrogen-containing polymers and one or more fatty acids are mixed to form a salt, and then the salt can be used as a component of the composition for forming a backcoat layer to prepare the composition for forming a backcoat layer. When the nitrogen-containing polymer and the fatty acids are mixed to form the ammonium salt of the alkyl ester anion represented by formula 1, the nitrogen atom constituting the nitrogen-containing polymer and the carboxyl group of the fatty acid may also react to form the following structure, and the form including such a structure is also included in the above compound.

[0105] [ka]

[0106] Examples of the fatty acids include fatty acids having an alkyl group as described above as R in formula 1 and fluorinated fatty acids having a fluorinated alkyl group as described above as R in formula 1.

[0107] The mixing ratio of the nitrogen-containing polymer and the fatty acid used to form the compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 is preferably 10:90 to 90:10, more preferably 20:80 to 85:15, and even more preferably 30:70 to 80:20, as the mass ratio of the nitrogen-containing polymer: the fatty acid. In addition, the compound having an ammonium salt structure of an alkyl ester anion represented by formula 1 can be used, for example, 1.0 to 20.0 parts by mass, and preferably 1.0 to 10.0 parts by mass, per 100.0 parts by mass of carbon black, when preparing the composition for forming a backcoat layer. In addition, for example, in preparing the composition for forming a backcoat layer, 0.1 to 10.0 parts by mass of the nitrogen-containing polymer can be used, and preferably 0.5 to 8.0 parts by mass of the nitrogen-containing polymer can be used, per 100.0 parts by mass of carbon black. The fatty acids can be used in an amount of, for example, 0.05 to 10.0 parts by mass, and preferably 0.1 to 5.0 parts by mass, per 100.0 parts by mass of carbon black.

[0108] Regarding the components that can be contained in the backcoat layer, the backcoat layer can include a binder and can also include additives. For the binder and additives of the backcoat layer, known techniques related to the backcoat layer can be applied, and known techniques related to the formulation of the magnetic layer and / or nonmagnetic layer can also be applied. For example, the descriptions of the backcoat layer can be referred to in paragraphs 0018-0020 of JP 2006-331625 A and in column 4, line 65 to column 5, line 38 of U.S. Patent No. 7,029,774.

[0109] <Various thicknesses> Regarding the thickness (total thickness) of the magnetic tape, with the enormous increase in the amount of information in recent years, there is a demand for magnetic recording media to have higher recording capacity (higher capacity). As a means for increasing the capacity of tape-shaped magnetic recording media (i.e., magnetic tape), there is the reduction in the thickness of the magnetic tape and the increase in the length of the magnetic tape contained in one magnetic tape cartridge. From this point of view, the thickness (total thickness) of the magnetic tape is preferably 5.6 μm or less, more preferably 5.5 μm or less, even more preferably 5.4 μm or less, even more preferably 5.3 μm or less, and even more preferably 5.2 μm or less. From the viewpoint of ease of handling, the thickness of the magnetic tape is preferably 3.0 μm or more, and more preferably 3.5 μm or more.

[0110] The thickness (total thickness) of the magnetic tape can be measured by the following method. Ten samples (e.g., 5 to 10 cm long) are cut out from any part of the magnetic tape, and the samples are stacked and the thickness is measured. The measured thickness is divided by 10 to obtain the value (thickness per sample), which is the total thickness. The thickness measurement can be performed using a known measuring device capable of measuring thickness to the order of 0.1 μm.

[0111] The thickness of the non-magnetic support is preferably 3.0 to 5.0 μm. The thickness of the magnetic layer can be optimized according to the saturation magnetization amount of the magnetic head used, the head gap length, the band of the recording signal, etc., and is generally 0.01 μm to 0.15 μm, and from the viewpoint of high-density recording, is preferably 0.02 μm to 0.12 μm, and more preferably 0.03 μm to 0.1 μm. At least one magnetic layer is sufficient, and the magnetic layer may be separated into two or more layers having different magnetic properties, and a known configuration related to a multilayer magnetic layer can be applied. When the magnetic layer is separated into two or more layers, the thickness of the magnetic layer is the total thickness of these layers. The thickness of the nonmagnetic layer is, for example, 0.1 to 1.5 μm, and preferably 0.1 to 1.0 μm. The thickness of the backcoat layer is preferably 0.9 μm or less, and more preferably 0.1 to 0.7 μm. Various thicknesses such as the thickness of the magnetic layer can be determined by the following method. A cross section of the magnetic tape in the thickness direction is exposed by an ion beam, and then the exposed cross section is observed by a scanning electron microscope. Various thicknesses can be obtained as the arithmetic average of thicknesses obtained at any two points in the cross section observation. Alternatively, various thicknesses can be obtained as design thicknesses calculated from manufacturing conditions, etc.

[0112] <Manufacturing process> (Preparation of compositions for forming each layer) The composition for forming the magnetic layer, non-magnetic layer or backcoat layer usually contains a solvent in addition to the various components described above. As the solvent, one or more of the various solvents usually used in the manufacture of coating-type magnetic recording media can be used. The solvent content of each layer-forming composition is not particularly limited. For the solvent, refer to paragraph 0153 of JP 2011-216149 A. The solid content concentration and solvent composition of each layer-forming composition may be appropriately adjusted according to the handling suitability of the composition, the coating conditions and the thickness of each layer to be formed. The process for preparing the composition for forming the magnetic layer, non-magnetic layer or backcoat layer usually includes at least a kneading process, a dispersing process, and a mixing process provided before or after these processes as necessary. Each individual process may be divided into two or more stages. The various components used in the preparation of each layer-forming composition may be added at the beginning or during any process. Also, each individual component may be added in two or more steps in a divided manner. For example, the binder may be added in a divided manner in the kneading process, the dispersing process and the mixing process for adjusting the viscosity after dispersion. In the manufacturing process of the magnetic tape, conventional known manufacturing techniques can be used as part of the process. In the kneading process, a device having a strong kneading force such as an open kneader, a continuous kneader, a pressure kneader, or an extruder can be used. Details of the kneading process are described in JP-A-1-106338 and JP-A-1-79274. As the dispersing machine, various known dispersing machines utilizing shear force such as a bead mill, a ball mill, a sand mill, or a homomixer can be used. Dispersing beads can be preferably used for dispersion. Examples of dispersing beads include ceramic beads and glass beads, and zirconia beads are preferred. Two or more types of beads may be used in combination. The bead diameter (particle size) and bead packing rate of the dispersing beads are not particularly limited and may be set according to the powder to be dispersed. Each layer-forming composition may be filtered by a known method before being subjected to the coating process. Filtration can be performed, for example, by filter filtration. As the filter used for filtration, for example, a filter with a pore size of 0.01 to 3 μm (for example, a glass fiber filter, a polypropylene filter, etc.) can be used.

[0113] (Coating process) The magnetic layer can be formed by directly applying the magnetic layer-forming composition onto the surface of the non-magnetic support, or by successively or simultaneously applying the magnetic layer-forming composition and the non-magnetic layer-forming composition in a multi-layer manner. The backcoat layer can be formed by applying the backcoat layer-forming composition onto the surface of the non-magnetic support opposite to the surface having the non-magnetic layer and / or magnetic layer (or the non-magnetic layer and / or magnetic layer will be provided later). For details of the coating for forming each layer, refer to paragraph 0066 of JP2010-231843A.

[0114] (Other processes) For other various steps for manufacturing the magnetic tape, known techniques can be applied. For various steps, for example, refer to paragraphs 0067 to 0070 of JP-A-2010-231843. For example, the coating layer of the magnetic layer-forming composition can be subjected to an orientation treatment in an orientation zone while the coating layer is in a wet state. For the orientation treatment, various known techniques including those described in paragraph 0052 of JP-A-2010-24113 can be applied. For example, the vertical orientation treatment can be performed by a known method such as a method using magnets with opposite poles facing each other. In the orientation zone, the drying speed of the coating layer can be controlled by the temperature and volume of the drying air and / or the transport speed in the orientation zone. In addition, the coating layer may be pre-dried before being transported to the orientation zone. As an example, the magnetic field strength in the vertical orientation treatment can be 0.1 to 1.5 T.

[0115] A long magnetic tape roll can be obtained by going through various processes. The obtained magnetic tape roll is cut (slit) to the width of the magnetic tape to be wound in the magnetic tape cartridge by a known cutting machine. The width is determined according to a standard and is usually 1 / 2 inch. 1 / 2 inch = 12.65 mm. A servo pattern is usually formed on the magnetic tape obtained by slitting. The servo pattern will be described in detail later. The magnetic tape is usually accommodated in a magnetic tape cartridge, and the magnetic tape cartridge is loaded into a magnetic tape device. In the magnetic tape cartridge, the magnetic tape is generally accommodated inside the cartridge body in a state where it is wound around a reel. The reel is rotatably provided inside the cartridge body. As the magnetic tape cartridge, a single-reel type magnetic tape cartridge having one reel inside the cartridge body and a twin-reel type magnetic tape cartridge having two reels inside the cartridge body are widely used. When a single-reel magnetic tape cartridge is loaded into a magnetic tape device for recording and / or reproducing data on the magnetic tape, the magnetic tape is pulled out from the magnetic tape cartridge and wound onto a reel on the magnetic tape device side. A magnetic head is disposed on the magnetic tape transport path from the magnetic tape cartridge to the take-up reel. The magnetic tape is fed out and wound up between the reel (supply reel) on the magnetic tape cartridge side and the reel (take-up reel) on the magnetic tape device side. During this time, the magnetic head comes into contact with and slides against the magnetic layer surface of the magnetic tape, thereby recording and / or reproducing data. In contrast, a dual-reel magnetic tape cartridge is equipped with both a supply reel and a take-up reel inside the magnetic tape cartridge.

[0116] (Formation of servo pattern) A servo pattern can be formed on the magnetic tape by a known method to enable tracking control of the magnetic head in the magnetic tape device, control of the running speed of the magnetic tape, etc. "Formation of a servo pattern" can also be called "recording of a servo signal." The servo signal is used to obtain dimensional information in the width direction of the magnetic tape while it is running, and the tension applied in the longitudinal direction of the magnetic tape is adjusted and changed according to the obtained dimensional information, thereby controlling the width direction of the magnetic tape.

[0117] The formation of the servo pattern will be described below.

[0118] The servo pattern is usually formed along the longitudinal direction of the magnetic tape. Methods of control using servo signals (servo control) include timing-based servo (TBS), amplitude servo, and frequency servo.

[0119] As shown in ECMA (European Computer Manufacturers Association)-319 (June 2001), magnetic tapes (generally called "LTO tapes") conforming to the LTO (Linear Tape-Open) standard employ a timing-based servo system. In this timing-based servo system, a servo pattern is formed by a pair of non-parallel magnetic stripes (also called "servo stripes") arranged continuously in the longitudinal direction of the magnetic tape. A servo system is a system that performs head tracking using a servo signal. In this invention and this specification, the "timing-based servo pattern" refers to a servo pattern that enables head tracking in a servo system of the timing-based servo system. As described above, the servo pattern is formed by a pair of non-parallel magnetic stripes in order to inform the servo signal reading element that passes over the servo pattern of its passing position. Specifically, the pair of magnetic stripes is formed so that the interval between them changes continuously along the width direction of the magnetic tape, and the servo signal reading element can know the relative position between the servo pattern and the servo signal reading element by reading the interval. This relative position information enables tracking of the data track. For this reason, a plurality of servo tracks are usually set on the servo pattern along the width direction of the magnetic tape.

[0120] A servo band is made up of a continuous servo pattern in the longitudinal direction of the magnetic tape. Usually, multiple servo bands are provided on a magnetic tape. For example, there are five servo bands on an LTO tape. The area between two adjacent servo bands is the data band. The data band is made up of multiple data tracks, and each data track corresponds to one servo track.

[0121] Also, in one embodiment, as shown in JP 2004-318983 A, information indicating the number of the servo band (also called "servo band ID (identification)" or "UDIM (Unique Data Band Identification Method) information") is embedded in each servo band. This servo band ID is recorded by shifting a specific one of a plurality of pairs of servo stripes in the servo band so that its position is displaced relatively in the longitudinal direction of the magnetic tape. Specifically, the way in which a specific one of a plurality of pairs of servo stripes is shifted is changed for each servo band. As a result, the recorded servo band ID is unique for each servo band, so that the servo band can be uniquely identified simply by reading one servo band with a servo signal reading element.

[0122] As a method for uniquely identifying servo bands, there is also a method using the staggered method as shown in ECMA-319 (June 2001). In this staggered method, a group of pairs of non-parallel magnetic stripes (servo stripes) arranged continuously in the longitudinal direction of the magnetic tape are recorded so that they are shifted in the longitudinal direction of the magnetic tape for each servo band. The combination of the shift between adjacent servo bands is unique across the entire magnetic tape, so when the servo pattern is read by two servo signal reading elements, it is possible to uniquely identify the servo bands.

[0123] Also, as specified in ECMA-319 (June 2001), information indicating the longitudinal position of the magnetic tape (also called "LPOS (Longitudinal Position) information") is usually embedded in each servo band. Like UDIM information, this LPOS information is also recorded by shifting the positions of a pair of servo stripes in the longitudinal direction of the magnetic tape. However, unlike UDIM information, the same signal is recorded in each servo band with this LPOS information.

[0124] It is also possible to embed information other than the above UDIM information and LPOS information in the servo bands. In this case, the embedded information may be different for each servo band, such as UDIM information, or may be common to all servo bands, such as LPOS information. Also, methods other than those described above can be used to embed information in the servo bands. For example, a predetermined code may be recorded by thinning out a predetermined pair from a group of pairs of servo stripes.

[0125] The head for forming a servo pattern is called a servo write head. The servo write head usually has a pair of gaps corresponding to the pair of magnetic stripes, the number of which is equal to the number of servo bands. Usually, a core and a coil are connected to each pair of gaps, and a magnetic field generated in the core can generate a leakage magnetic field in the pair of gaps by supplying a current pulse to the coil. When forming a servo pattern, a magnetic pattern corresponding to the pair of gaps can be transferred to the magnetic tape by inputting a current pulse while running the magnetic tape on the servo write head, thereby forming the servo pattern. The width of each gap can be appropriately set according to the density of the servo pattern to be formed. The width of each gap can be set, for example, to 1 μm or less, 1 to 10 μm, or 10 μm or more.

[0126] Before forming a servo pattern on the magnetic tape, the magnetic tape is usually subjected to a demagnetization (erase) process. This erase process can be performed by applying a uniform magnetic field to the magnetic tape using a direct current magnet or an alternating current magnet. There are two types of erase processes: DC (Direct Current) erase and AC (Alternating Current) erase. AC erase is performed by gradually lowering the strength of the magnetic field applied to the magnetic tape while reversing the direction of the magnetic field. On the other hand, DC erase is performed by applying a unidirectional magnetic field to the magnetic tape. There are two more methods of DC erase. The first method is horizontal DC erase, which applies a unidirectional magnetic field along the longitudinal direction of the magnetic tape. The second method is vertical DC erase, which applies a unidirectional magnetic field along the thickness direction of the magnetic tape. The erase process may be performed on the entire magnetic tape, or may be performed for each servo band of the magnetic tape.

[0127] The direction of the magnetic field of the formed servo pattern is determined according to the direction of erasure. For example, when the magnetic tape is subjected to horizontal DC erasure, the servo pattern is formed so that the direction of the magnetic field is opposite to the direction of erasure. This makes it possible to increase the output of the servo signal obtained by reading the servo pattern. As shown in JP2012-53940A, when the magnetic pattern is transferred to the magnetic tape that has been vertically DC erased using the above gap, the servo signal obtained by reading the formed servo pattern has a unipolar pulse shape. On the other hand, when the magnetic pattern is transferred to the magnetic tape that has been horizontally DC erased using the above gap, the servo signal obtained by reading the formed servo pattern has a bipolar pulse shape.

[0128] [Magnetic head] In the present invention and this specification, the term "magnetic tape device" refers to a device capable of at least one of recording data on a magnetic tape and reproducing data recorded on the magnetic tape. Such a device is generally called a drive. The magnetic head included in the magnetic tape device can be a recording head capable of recording data on a magnetic tape, and can also be a reproducing head capable of reproducing data recorded on the magnetic tape. In one embodiment, the magnetic tape device can include both a recording head and a reproducing head as separate magnetic heads. In another embodiment, the magnetic head included in the magnetic tape device can have a configuration in which both a recording element and a reproducing element are provided in one magnetic head. As the reproducing head, a magnetic head (MR head) including a magnetoresistive (MR) element capable of reading information recorded on a magnetic tape with good sensitivity as a reproducing element is preferable. As the MR head, various known MR heads (for example, a GMR (Giant Magnetoresistive) head, a TMR (Tunnel Magnetoresistive) head, etc.) can be used. In addition, the magnetic head that records and / or reproduces data may include a servo pattern reading element. Alternatively, the magnetic tape device may include a magnetic head (servo head) equipped with a servo pattern reading element as a head separate from the magnetic head that records and / or reproduces data. For example, a magnetic head that records and / or reproduces recorded data (hereinafter also referred to as a "recording and reproducing head") may include two servo signal reading elements, and each of the two servo signal reading elements may simultaneously read two adjacent servo bands sandwiching a data band. One or more data elements may be disposed between the two servo signal reading elements. The element for recording data (recording element) and the element for reproducing data (reproducing element) are collectively referred to as the "data element."

[0129] By using a reproducing element with a narrow reproducing element width as the reproducing element to reproduce data, data recorded at a high density can be reproduced with high sensitivity. From this viewpoint, the reproducing element width of the reproducing element is preferably 0.8 μm or less. The reproducing element width of the reproducing element can be, for example, 0.3 μm or more. However, from the above viewpoint, it is also preferable that the reproducing element width is less than this value. On the other hand, the narrower the reproducing element width, the more likely it is that phenomena such as poor reproduction caused by off-track will occur. In order to suppress the occurrence of such phenomena, a magnetic tape device is preferred that controls the dimension of the magnetic tape in the width direction by adjusting and changing the tension applied to the magnetic tape in the longitudinal direction while it is running. Here, the "reading element width" refers to the physical dimension of the reading element width. Such physical dimension can be measured using an optical microscope, a scanning electron microscope, or the like.

[0130] When recording data and / or reproducing recorded data, head tracking using servo signals can be performed first. That is, by making the servo signal reading element follow a specific servo track, the data element can be controlled to pass over the target data track. The data track is moved by changing the servo track read by the servo signal reading element in the tape width direction. The recording / reproducing head can also record and / or reproduce data on other data bands by using the UDIM information described above to move the servo signal reading element to a specific servo band and start tracking on that servo band.

[0131] FIG. 2 shows an example of the arrangement of data bands and servo bands. In FIG. 2, a plurality of servo bands 1 are arranged on the magnetic layer of the magnetic tape MT, sandwiched between guide bands 3. A plurality of regions 2 sandwiched between two servo bands are data bands. A servo pattern is a magnetized region, and is formed by magnetizing a specific region of the magnetic layer with a servo write head. The region magnetized by the servo write head (the position where the servo pattern is formed) is determined by a standard. For example, in an LTO Ultrium format tape, which is an industry standard, a plurality of servo patterns inclined with respect to the tape width direction are formed on the servo band during the manufacturing of the magnetic tape, as shown in FIG. 3. More specifically, in FIG. 3, a servo frame SF on the servo band 1 is composed of a servo subframe 1 (SSF1) and a servo subframe 2 (SSF2). The servo subframe 1 is composed of an A burst (symbol A in FIG. 3) and a B burst (symbol B in FIG. 3). The A burst is composed of servo patterns A1 to A5, and the B burst is composed of servo patterns B1 to B5. On the other hand, the servo subframe 2 is composed of a C burst (symbol C in FIG. 3) and a D burst (symbol D in FIG. 3). The C burst is composed of servo patterns C1 to C4, and the D burst is composed of servo patterns D1 to D4. Such 18 servo patterns are arranged in a subframe arranged in a 5, 5, 4, 4 arrangement in a set of 5 and 4, and are used to identify a servo frame. For the sake of explanation, one servo frame is shown in FIG. 3. However, in reality, a plurality of servo frames are arranged in the running direction in each servo band on the magnetic layer of a magnetic tape where head tracking of the timing-based servo method is performed. In FIG. 3, the arrow indicates the running direction. For example, an LTO Ultrium format tape usually has 5,000 or more servo frames per meter of tape length in each servo band on the magnetic layer. EXAMPLES

[0132] The present invention will be described below based on examples. However, the present invention is not limited to the embodiments shown in the examples. The indications of "parts" and "%" below refer to "parts by mass" and "% by mass" unless otherwise specified. Furthermore, the steps and evaluations described below were carried out in an environment with an atmospheric temperature of 23°C ± 1°C unless otherwise specified. Furthermore, "eq" described below refers to equivalent, which is a unit that cannot be converted into the SI unit system.

[0133] [Nonmagnetic support] In Table 1, "PEN" indicates a polyethylene naphthalate substrate and "PET" indicates a polyethylene terephthalate substrate.

[0134] [Ferromagnetic powder] In Table 1 described later, "BaFe" in the column for the type of ferromagnetic powder indicates hexagonal barium ferrite powder having an average particle size (average plate diameter) of 21 nm.

[0135] In Table 1, "SrFe1" in the column for type of ferromagnetic powder indicates a hexagonal strontium ferrite powder prepared as follows. 1707 g of SrCO3, 687 g of H3BO3, 1120 g of Fe2O3, 45 g of Al(OH)3, 24 g of BaCO3, 13 g of CaCO3, and 235 g of Nd2O3 were weighed out and mixed in a mixer to obtain a raw material mixture. The obtained raw material mixture was melted in a platinum crucible at a melting temperature of 1390°C, and the melt was poured into a rod shape at about 6 g / sec by heating the tapping hole at the bottom of the platinum crucible while stirring the melt. The tapped liquid was rolled and quenched with a water-cooled twin roller to produce an amorphous body. 280 g of the produced amorphous body was placed in an electric furnace, heated to 635°C (crystallization temperature) at a heating rate of 3.5°C / min, and held at that temperature for 5 hours to precipitate (crystallize) hexagonal strontium ferrite particles. Next, the crystallized material obtained above containing hexagonal strontium ferrite particles was coarsely crushed in a mortar, and 1000 g of zirconia beads with a particle size of 1 mm and 800 mL of 1% aqueous acetic acid solution were added to a glass bottle and dispersed for 3 hours using a paint shaker. The resulting dispersion was then separated from the beads and placed in a stainless steel beaker. The dispersion was left to stand at a liquid temperature of 100°C for 3 hours to dissolve the glass components, and then precipitated in a centrifuge and washed by repeated decantation, and dried for 6 hours in a heating furnace at a furnace temperature of 110°C to obtain hexagonal strontium ferrite powder. The average particle size of the hexagonal strontium ferrite powder obtained above is 18 nm, and the activation volume is 902 nm. 3 , the anisotropy constant Ku is 2.2×10 5 J / m 3 , mass magnetization σs is 49A m 2 / kg. A 12 mg sample powder was taken from the hexagonal strontium ferrite powder obtained above, and this sample powder was partially dissolved under the dissolution conditions exemplified above. The elemental analysis of the filtrate obtained was performed using an ICP analyzer to determine the surface layer content of neodymium atoms. Separately, 12 mg of sample powder was taken from the hexagonal strontium ferrite powder obtained above, and this sample powder was completely dissolved under the dissolution conditions exemplified above. The elemental analysis of the filtrate obtained was performed using an ICP analyzer to determine the bulk content of neodymium atoms. The neodymium atom content (bulk content) relative to 100 atomic % of iron atoms in the hexagonal strontium ferrite powder obtained above was 2.9 atomic %. The surface layer content of neodymium atoms was 8.0 atomic %. The ratio of the surface layer content to the bulk content, "surface layer content / bulk content," was 2.8, confirming that neodymium atoms were unevenly distributed in the surface layers of the particles.

[0136] It was confirmed that the powder obtained above exhibited a hexagonal ferrite crystal structure by scanning with CuKα radiation at a voltage of 45 kV and an intensity of 40 mA and measuring the X-ray diffraction pattern under the following conditions (X-ray diffraction analysis). The powder obtained above exhibited a magnetoplumbite-type (M-type) hexagonal ferrite crystal structure. The crystal phase detected by the X-ray diffraction analysis was a single phase of magnetoplumbite type. PANalytical X'Pert Pro diffractometer, PIXcel detector Soller slits for incident and diffracted beams: 0.017 radians Dispersion slit fixed angle: 1 / 4 degree Mask: 10mm Anti-scatter slit: 1 / 4 degree Measurement mode: Continuous Measurement time per step: 3 seconds Measurement speed: 0.017 degrees per second Measurement step: 0.05 degrees

[0137] In Table 1, "SrFe2" in the column for type of ferromagnetic powder indicates hexagonal strontium ferrite powder prepared as follows. 1725 g of SrCO3, 666 g of H3BO3, 1332 g of Fe2O3, 52 g of Al(OH)3, 34 g of CaCO3, and 141 g of BaCO3 were weighed out and mixed in a mixer to obtain a raw material mixture. The obtained raw material mixture was melted in a platinum crucible at a melting temperature of 1380°C, and the melt was poured into a rod shape at about 6 g / sec by heating the tapping hole at the bottom of the platinum crucible while stirring the melt. The tapped liquid was rolled and quenched with a water-cooled twin roll to produce an amorphous body. 280 g of the obtained amorphous body was placed in an electric furnace, heated to 645° C. (crystallization temperature), and held at that temperature for 5 hours to precipitate (crystallize) hexagonal strontium ferrite particles. Next, the crystallized material obtained above containing hexagonal strontium ferrite particles was coarsely crushed in a mortar, and 1000 g of zirconia beads with a particle size of 1 mm and 800 mL of 1% aqueous acetic acid solution were added to a glass bottle and dispersed for 3 hours using a paint shaker. The resulting dispersion was then separated from the beads and placed in a stainless steel beaker. The dispersion was left to stand at a liquid temperature of 100°C for 3 hours to dissolve the glass components, and then precipitated in a centrifuge and washed by repeated decantation, and dried for 6 hours in a heating furnace at a furnace temperature of 110°C to obtain hexagonal strontium ferrite powder. The average particle size of the obtained hexagonal strontium ferrite powder was 19 nm, and the activation volume was 1102 nm. 3 , the anisotropy constant Ku is 2.0×10 5 J / m 3 , mass magnetization σs is 50A m 2 / kg.

[0138] In Table 1, "ε-iron oxide" in the column for type of ferromagnetic powder indicates ε-iron oxide powder prepared as follows. 8.3g of iron (III) nitrate nonahydrate, 1.3g of gallium (III) nitrate octahydrate, 190mg of cobalt (II) nitrate hexahydrate, 150mg of titanium (IV) sulfate, and 1.5g of polyvinylpyrrolidone (PVP) were dissolved in 90g of pure water, and 4.0g of ammonia solution with a concentration of 25% was added under the condition of an atmospheric temperature of 25°C while stirring with a magnetic stirrer in the air, and the mixture was stirred for 2 hours at an atmospheric temperature of 25°C. A citric acid solution obtained by dissolving 1g of citric acid in 9g of pure water was added to the obtained solution, and the mixture was stirred for 1 hour. The powder precipitated after stirring was collected by centrifugation, washed with pure water, and dried in a heating furnace at an internal temperature of 80°C. 800g of pure water was added to the dried powder, and the powder was dispersed in water again to obtain a dispersion. The obtained dispersion was heated to 50°C, and 40g of 25% ammonia aqueous solution was added dropwise while stirring. After stirring for 1 hour while maintaining the temperature at 50°C, 14mL of tetraethoxysilane (TEOS) was added dropwise and stirred for 24 hours. 50g of ammonium sulfate was added to the obtained reaction solution, and the precipitated powder was collected by centrifugation, washed with pure water, and dried for 24 hours in a heating furnace with an internal temperature of 80°C to obtain a precursor of ferromagnetic powder. The obtained precursor of the ferromagnetic powder was placed in a heating furnace at an internal temperature of 1000° C. in an air atmosphere and subjected to a heat treatment for 4 hours. The heat-treated ferromagnetic powder precursor was placed in a 4 mol / L aqueous solution of sodium hydroxide (NaOH), and the liquid temperature was maintained at 70°C while stirring for 24 hours, thereby removing impurities such as silicate compounds from the heat-treated ferromagnetic powder precursor. Thereafter, the silicic acid compound was removed by centrifugation, and the ferromagnetic powder was collected and washed with pure water to obtain a ferromagnetic powder. The composition of the obtained ferromagnetic powder was confirmed by inductively coupled plasma-optical emission spectrometry (ICP-OES). The results showed that the powder was composed of Ga, Co, and Ti substituted ε-iron oxide (ε-Ga 0.28 Co 0.05 Ti 0.05 Fe 1.62 In addition, X-ray diffraction analysis was performed under the same conditions as those described above for the hexagonal strontium ferrite powder SrFe1, and it was confirmed from the peaks in the X-ray diffraction pattern that the obtained ferromagnetic powder had a single-phase ε-phase crystal structure (ε-iron oxide type crystal structure) that did not contain α-phase or γ-phase crystal structures. The average particle size of the obtained ε-iron oxide powder was 12 nm, and the activation volume was 746 nm. 3 , the anisotropy constant Ku is 1.2×10 5 J / m 3 , mass magnetization σs is 16A m 2 / kg.

[0139] The activation volume and anisotropy constant Ku of the above hexagonal strontium ferrite powder and ε-iron oxide powder were determined for each ferromagnetic powder by the method described above using a vibrating sample magnetometer (manufactured by Toei Kogyo Co., Ltd.). The mass magnetization σs is a value measured using a vibrating sample magnetometer (manufactured by Toei Industry Co., Ltd.) at a magnetic field strength of 1194 kA / m (15 kOe).

[0140] [Example 1] (1) Formulation of the composition for forming the magnetic layer (Magnetic liquid) Ferromagnetic powder (see Table 1): 100.0 parts SO3Na group-containing polyurethane resin: 14.0 parts Weight average molecular weight: 70,000, SO3Na group: 0.4meq / g Cyclohexanone: 150 parts Methyl ethyl ketone: 150 parts (Abrasive Liquid A) Alumina abrasive (average particle size: 100 nm): 3.0 parts Sulfonic acid group-containing polyurethane resin: 0.3 parts Weight average molecular weight: 70,000, SO3Na group: 0.3meq / g Cyclohexanone: 26.7 parts (Abrasive liquid B) Diamond abrasive (average particle size: 100 nm): 1.0 part Sulfonic acid group-containing polyurethane resin: 0.1 parts Weight average molecular weight: 70,000, SO3Na group: 0.3meq / g Cyclohexanone: 26.7 parts (Silica sol) Colloidal silica (average particle size: 100 nm): 0.2 parts Methyl ethyl ketone: 1.4 parts (Other Ingredients) Stearic acid: 2.0 parts Butyl stearate: 10.0 parts Polyisocyanate (Coronate, manufactured by Nippon Polyurethane Co., Ltd.): 2.5 parts Cyclohexanone: 200.0 parts Methyl ethyl ketone: 200.0 parts

[0141] (2) Formulation of the composition for forming the nonmagnetic layer Non-magnetic inorganic powder (α-iron oxide): 100.0 parts Average particle size (average major axis length): 10nm Average acicular ratio: 1.9 BET (Brunauer-Emmett-Teller) specific surface area: 75m 2 / g Carbon black: 25.0 parts Average particle size: 20nm SO3Na group-containing polyurethane resin: 18 parts Weight average molecular weight: 70,000, SO3Na group: 0.2meq / g Stearic acid: 1.0 parts Cyclohexanone: 300.0 parts Methyl ethyl ketone: 300.0 parts

[0142] (3) Formulation of the composition for forming the backcoat layer Carbon black: 100.0 parts Cabot BP-800, average particle size: 17 nm SO3Na group-containing polyurethane resin (SO3Na group: 70eq / ton): 20.0 parts Vinyl chloride resin containing OSO3K group (OSO3K group: 70eq / ton): 30.0 parts Polyethyleneimine (manufactured by Nippon Shokubai, number average molecular weight 600): See Table 1 Stearic acid: see Table 1 Cyclohexanone: 140.0 parts Methyl ethyl ketone: 170.0 parts Butyl stearate: 2.0 parts Stearic acid amide: 0.1 parts

[0143] (4) Manufacturing of magnetic tapes and magnetic tape cartridges The above components of the magnetic liquid were dispersed for 24 hours using a batch-type vertical sand mill to prepare the magnetic liquid. Zirconia beads with a diameter of 0.5 mm were used as the dispersion beads. Regarding the polishing compound liquids, the above-mentioned components of polishing compound liquid A and polishing compound liquid B were dispersed for 24 hours using a batch-type ultrasonic device (20 kHz, 300 W) to obtain polishing compound liquid A and polishing compound liquid B, respectively. The magnetic liquid, abrasive liquid A, and abrasive liquid B were mixed with the above-mentioned silica sol and other components, and then dispersed for 30 minutes using a batch-type ultrasonic device (20 kHz, 300 W).The mixture was then filtered using a filter with a pore size of 0.5 μm to prepare a magnetic layer-forming composition. The non-magnetic layer-forming composition was prepared by dispersing the above components for 24 hours using a batch-type vertical sand mill. Zirconia beads with a bead diameter of 0.1 mm were used as the dispersion beads. The obtained dispersion was filtered using a filter with a pore size of 0.5 μm to prepare the non-magnetic layer-forming composition. The composition for forming a backcoat layer is prepared by kneading the above-mentioned components with a continuous kneader, and then dispersing them with a sand mill. 40.0 parts of polyisocyanate (Coronate L manufactured by Nippon Polyurethane Industry Co., Ltd.) and 1000.0 parts of methyl ethyl ketone are added to the obtained dispersion, and then filtering is performed with a filter having a pore size of 1 μm to prepare a composition for forming a backcoat layer. The composition for forming a nonmagnetic layer prepared above was applied onto the surface of a 4.1 μm thick support of the type shown in Table 1, and then dried to a dry thickness of 0.7 μm, thereby forming a nonmagnetic layer. Next, the magnetic layer-forming composition prepared above was applied onto the non-magnetic layer so as to give a coating layer with a thickness of 0.1 μm after drying. Thereafter, while the coating layer of the magnetic layer-forming composition was still wet, a magnetic field with a strength of 0.3 T was applied perpendicularly to the surface of the coating layer to perform a vertical alignment treatment, followed by drying to form a magnetic layer. Thereafter, the backcoat layer-forming composition prepared above was applied to the surface of the support opposite to the surface on which the nonmagnetic layer and magnetic layer were formed, and then dried to form a backcoat layer with a thickness of 0.3 μm after drying. Thereafter, a surface smoothing treatment (calendering) was performed using a calender roll consisting only of a metal roll at a speed of 100 m / min, a linear pressure of 300 kg / cm, and a calender temperature (surface temperature of the calender roll) of 90° C. In this manner, a long magnetic tape raw sheet was obtained. After that, the magnetic tape was heat-treated for 36 hours in an atmosphere temperature of 70°C, and then the long magnetic tape was slit into 1 / 2 inch widths to obtain a magnetic tape. A servo signal was recorded on the magnetic layer of the obtained magnetic tape using a commercially available servo writer, thereby obtaining a magnetic tape having a servo pattern (timing-based servo pattern) arranged in accordance with the LTO (Linear Tape-Open) Ultrium format. After the servo pattern was formed, the magnetic tape (970 m long) was wound onto the cartridge reel of a magnetic tape cartridge (LTO Ultrium 7 data cartridge) to the final product length (960 m), and the remaining 10 m was cut off. A leader tape conforming to item 9 of Standard ECMA (European Computer Manufacturers Association)-319 (June 2001) Section 3 was spliced ​​to the end of the cut off piece using a commercially available splicing tape. As a result of the above, a single-reel type magnetic tape cartridge of Example 1 was produced, in which a magnetic tape having a length of 960 m was wound around a cartridge reel.

[0144] Whether the backcoat layer of a magnetic tape contains a compound containing an ammonium salt structure of an alkyl ester anion represented by formula 1, which is formed from polyethyleneimine and stearic acid, can be confirmed by the following method. A sample is cut out from the magnetic tape, and the surface of the backcoat layer (measurement area: 300 μm × 700 μm) is subjected to X-ray photoelectron spectroscopy using an ESCA device. In detail, a wide scan measurement is performed using the ESCA device under the following measurement conditions. In the measurement results, peaks are confirmed at the position of the binding energy of the ester anion and the position of the binding energy of the ammonium cation. Equipment: Shimadzu AXIS-ULTRA Excitation X-ray source: Monochromated Al-Kα radiation Scan range: 0~1200eV Pass energy: 160 eV Energy resolution: 1eV / step Acquisition time: 100ms / step Number of times: 5 In addition, a sample piece of 3 cm in length was cut out from the magnetic tape, and the surface of the backcoat layer was measured with an ATR-FT-IR (Attenuated total reflection-Fourier transform-infrared spectrometer) (reflection method). - The wave number corresponding to the absorption of -1 or 1430cm -1 ), and the wavenumber corresponding to the absorption of the ammonium cation (2400 cm -1 ) absorption is confirmed.

[0145] The above steps were repeated to prepare three magnetic tape cartridges. One magnetic tape cartridge was used for (5) to (7) below, another magnetic tape cartridge was used for (8) and (9) below, and the remaining magnetic tape cartridge was used for evaluating the running stability described below.

[0146] (5) Recording of data on magnetic tapes before storage and playback of recorded data Recording and playback before storage were performed using a magnetic tape device with the configuration shown in Figure 1. The recording and playback head mounted on the recording and playback head unit has 32 or more channels of playback elements (playback element width: 0.8 μm) and recording elements, with servo signal reading and playback elements on both sides. To acclimate the magnetic tape cartridge to the recording and playback environment, the cartridge was placed in an environment with an ambient temperature of 23° C. and a relative humidity of 50% for five days. After that, recording and playback were performed in the same environment as described below. A magnetic tape cartridge is set in a magnetic tape device and the magnetic tape is loaded. Next, while performing servo tracking, pseudo-random data with a specific data pattern is recorded on the magnetic tape by the recording / playback head unit. A constant tension of 0.50 N is applied to the tape in the longitudinal direction during this process. At the same time as the data is recorded, the servo band intervals over the entire length of the tape are measured every 1 m along the longitudinal direction and recorded in the cartridge memory. Next, the data recorded on the magnetic tape is reproduced by the recording / reproducing head unit while performing servo tracking. At the same time as reproduction, the value of the servo band interval is measured, and based on the information recorded in the cartridge memory, the tension applied in the longitudinal direction of the tape is changed so that the absolute value of the difference from the servo band interval at the time of recording at the same longitudinal position approaches 0. During reproduction, the measurement of the servo band interval and the tension control based on the measurement are performed continuously in real time. During such reproduction, the tension applied in the longitudinal direction of the magnetic tape is changed in the range of 0.50N to 0.85N by the control device of the magnetic tape device. Therefore, during the above reproduction, the maximum value of the tension applied in the longitudinal direction of the magnetic tape is 0.85N. At the end of the playback, the entire length of the magnetic tape has been wound onto the cartridge reel of the magnetic tape cartridge.

[0147] (6) Winding (rewinding) onto cartridge reels and storage The magnetic tape was then run in the magnetic tape device under the above-mentioned environment until the entire length of the magnetic tape was wound onto the take-up reel of the magnetic tape device. The tension applied to the magnetic tape in the longitudinal direction during the winding was set to a constant value of 0.50 N. Thereafter, a constant tension shown in Table 1 was applied to the magnetic tape in the longitudinal direction, and the entire length of the magnetic tape was wound onto a cartridge reel (also referred to as "rewinding"). After the above-mentioned rewinding, the magnetic tape cartridge containing the magnetic tape was stored in an environment with an ambient temperature of 60° C. and a relative humidity of 20% for 24 hours. The inventors speculate that this storage may be equivalent to a long-term storage of about 10 years at an ambient temperature of 32° C. and a relative humidity of 55%.

[0148] (7) Evaluation of recording and playback quality after storage After the above storage, the magnetic tape cartridge was placed in an environment with an ambient temperature of 23°C and a relative humidity of 50% for 5 days to allow it to acclimate to the environment in which it would be played back. Thereafter, in the same environment, playback was performed in the same manner as in the playback before storage in (5) above. That is, playback was performed while changing the tension applied to the magnetic tape in the longitudinal direction as described above. The number of channels in the above playback was 32. When the data for all 32 channels was read correctly during playback after storage, the recording and playback quality was rated as "3." When the data for channels 31 to 28 was read correctly, the recording and playback quality was rated as "2." In all other cases, the recording and playback quality was rated as "1."

[0149] (8) The number of depressions on the surface of the magnetic layer having a circle-equivalent diameter of 0.20 μm or more and 0.50 μm or less (per 40 μm × 40 μm area) The following conditions were used as the AFM measurement conditions, and the number of dents having an equivalent circle diameter within the above range (per area of ​​40 μm×40 μm) was determined for the magnetic layer surface of the magnetic tape by the method described above. An AFM (BRUKER Nanoscope 5) is used in peak force tapping mode to measure an area of ​​40 μm × 40 μm on the surface of the magnetic layer of the magnetic tape. A BRUKER SCANASYST-AIR probe is used, with a resolution of 512 pixels × 512 pixels and a scan speed of 512 seconds per screen (512 pixels × 512 pixels).

[0150] (9) Total thickness of magnetic tape (tape thickness) Ten tape samples (5 cm long) were cut out from any part of the magnetic tape, and the tape samples were stacked to measure the thickness. The thickness was measured using a digital thickness meter with a Millimar 1240 compact amplifier and a Millimar 1301 inductive probe manufactured by MARH. The measured thickness was divided by 10 to obtain the value (thickness per tape sample), which was taken as the tape thickness. The tape thickness of the magnetic tape was 5.2 μm. The tape thickness was also measured in the examples and comparative examples described below, and all of them had a tape thickness of 5.2 μm.

[0151] [Examples 2 to 16, Comparative Examples 1 to 3、5~9、11、12、19、 20] A magnetic tape cartridge was produced and various evaluations were carried out in the same manner as in Example 1, except that the items in Table 1 were changed as shown in Table 1. In the examples and comparative examples in Table 1 where the "Tension change during running" column is marked "Yes," playback before storage was performed by changing the tension applied to the magnetic tape in the longitudinal direction within the same minimum to maximum range as in Example 1. In the examples in Table 1 where "none" is listed in the "tension change during running" column, playback before storage was performed with a constant tension of 0.50 N applied in the longitudinal direction of the magnetic tape. In the examples and comparative examples, the playback after storage was performed in the same manner as the playback before storage. That is, the tension applied in the longitudinal direction of the magnetic tape during playback after storage and the presence or absence of change in the tension were the same as those before storage. For the examples and comparative examples in which the tension values ​​are listed in the "Rewinding Tension" column in Table 1, the tension applied in the longitudinal direction of the magnetic tape when winding (rewinding) onto the cartridge reel in (6) above was the value shown in Table 1. For the comparative examples in Table 1 where the "Rewinding tension" column states "No rewinding," after playback as described above in (5), the magnetic tape cartridge containing the magnetic tape was stored for 24 hours in an environment with an ambient temperature of 60°C and a relative humidity of 20% without rewinding.

[0152] [Evaluation of running stability when winding onto a cartridge reel with tension of 0.40N or less] For each of the magnetic tape cartridges of the examples and comparative examples, the running stability during winding onto the cartridge reel at a tension of 0.40 N or less was evaluated using a magnetic tape device having the configuration shown in FIG. To acclimate the magnetic tape cartridge to the environment for evaluation, the cartridge was placed in an environment with an ambient temperature of 23° C. and a relative humidity of 50% for five days. After that, the cartridge was evaluated in the same environment as follows. A magnetic tape cartridge is set in a magnetic tape device, and the magnetic tape is loaded. Next, the entire length of the magnetic tape is wound onto the take-up reel of the magnetic tape device while adjusting the tension in the same way as during playback in Example 1. Thereafter, a constant tension of 0.40 N is applied in the longitudinal direction of the magnetic tape in the same way as in the rewinding in Example 1, and the entire length of the magnetic tape is wound onto the cartridge reel (rewinding). During this rewinding, the edge position fluctuation amount (unit: μm) in the tape width direction of the edges on both sides of the magnetic tape is measured by a measuring device (device body: MTI-2000 Fotonic Sensor (manufactured by MTI Instruments Inc.), lower detection limit of the probe position fluctuation amount: 10 μm) installed outside the magnetic tape cartridge. When an edge position fluctuation of 300 μm or more occurs on at least one edge, it is evaluated as "B", and when no such edge position fluctuation occurs, it is evaluated as "A". In the case of evaluation result "B", the inventor believes that there is a possibility that edge damage may occur in the magnetic tape cartridge after rewinding.

[0153] The above results are shown in Table 1 (Table 1-1 and Table 1-2).

[0154] [Table 1-1]

[0155] [Table 1-2]

[0156] From the results shown in Table 1, it can be confirmed that in the embodiment, the magnetic tape was able to run stably when stored in the magnetic tape cartridge, and good recording and playback quality was obtained after storage.

[0157] A magnetic tape cartridge was produced in the same manner as in Example 1, except that no vertical orientation treatment was performed during the production of the magnetic tape. A sample piece was cut out from the magnetic tape removed from the magnetic tape cartridge. The squareness in the vertical direction of the sample piece was measured by the above-mentioned method using a vibrating sample magnetometer, TM-TRVSM5050-SMSL model manufactured by Tamagawa Seisakusho, and was found to be 0.55. The magnetic tape was also removed from the magnetic tape cartridge of Example 1, and a sample piece was cut out from this magnetic tape. The squareness ratio in the vertical direction was similarly determined to be 0.60.

[0158] The magnetic tapes taken out of the two magnetic tape cartridges were each attached to a 1 / 2 inch reel tester, and the electromagnetic conversion characteristics (SNR; Signal-to-Noise Ratio) were evaluated by the following method. As a result, the magnetic tape taken out of the magnetic tape cartridge of Example 1 had an SNR value 2 dB higher than that of the magnetic tape produced without the vertical orientation treatment. In an environment with a temperature of 23°C and a relative humidity of 50%, 10 passes of recording and reproduction were performed with a tension of 0.7 N applied in the longitudinal direction of the magnetic tape. The relative speed between the magnetic tape and the magnetic head was 6 m / sec. Recording was performed using a MIG (Metal-in-gap) head (gap length 0.15 μm, track width 1.0 μm) as the recording head, and the recording current was set to the optimal recording current for each magnetic tape. Reproduction was performed using a GMR (Giant-magnetoresistive) head (element thickness 15 nm, shield spacing 0.1 μm, reproduction element width 0.8 μm) as the reproduction head. A signal with a linear recording density of 300 kfci was recorded, and the reproduction signal was measured with a spectrum analyzer manufactured by Shibasoku. The unit kfci is the unit of linear recording density (not convertible to SI units). The signal was used at a portion where the signal was sufficiently stable after the magnetic tape started running. [Industrial Applicability]

[0159] One aspect of the present invention is useful in the technical fields of various data storage such as archives.

Claims

1. A take-up reel; A magnetic tape; a magnetic tape cartridge having a cartridge reel; A magnetic tape device comprising: The magnetic tape device includes: the magnetic tape is run between the take-up reel and the cartridge reel under tension in the longitudinal direction of the magnetic tape, the maximum value of the tension being 0.50 N or more; the magnetic tape after being run under the tension is wound around the cartridge reel under a tension of 0.40 N or less in the longitudinal direction of the magnetic tape; The magnetic tape has a non-magnetic support and a magnetic layer containing a ferromagnetic powder; A magnetic tape device, wherein the number of depressions having a circle-equivalent diameter of 0.20 μm or more and 0.50 μm or less present on the surface of the magnetic layer is 10 to 500 per area of ​​40 μm×40 μm.

2. 2. The magnetic tape device according to claim 1, wherein tension applied to the magnetic tape in the longitudinal direction during the running is changed.

3. 3. The magnetic tape device according to claim 1, wherein the magnetic tape has a thickness of 5.2 [mu]m or less.

4. 4. The magnetic tape device according to claim 1, wherein the magnetic tape further comprises a non-magnetic layer containing non-magnetic powder between the non-magnetic support and the magnetic layer.

5. 5. The magnetic tape device according to claim 1, wherein the magnetic tape further comprises a backcoat layer containing a nonmagnetic powder on a surface side of the nonmagnetic support opposite to the surface side having the magnetic layer.

6. 6. The magnetic tape device according to claim 5, wherein the non-magnetic powder in the backcoat layer includes carbon black.

7. 7. The magnetic tape device according to claim 1, wherein the squareness ratio of the magnetic tape in the perpendicular direction is 0.60 or more.

8. The magnetic tape is run between the take-up reel and the cartridge reel of the magnetic tape cartridge under tension in the longitudinal direction of the magnetic tape, the maximum value of the tension being 0.50 N or more, and A magnetic tape used in a magnetic tape device that applies a tension of 0.40 N or less in a longitudinal direction of the magnetic tape after the magnetic tape has been run under the tension, and winds the magnetic tape around the cartridge reel, A non-magnetic support and a magnetic layer containing ferromagnetic powder, a backcoat layer containing a nonmagnetic powder on the surface side of the nonmagnetic support opposite to the surface side having the magnetic layer, the number of depressions having a circle-equivalent diameter of 0.20 μm or more and 0.50 μm or less present on the surface of the magnetic layer is 10 or more and 500 or less per an area of ​​40 μm×40 μm; and The backcoat layer contains a compound having an ammonium salt structure of an alkyl ester anion represented by the following formula 1: 【Chemistry 1】 A magnetic tape, wherein in formula 1, R represents an alkyl group having 7 or more carbon atoms or a fluorinated alkyl group having 7 or more carbon atoms, and Z + represents an ammonium cation.

9. 9. The magnetic tape according to claim 8, wherein tension applied to the magnetic tape in the longitudinal direction is changed during the running.

10. 10. The magnetic tape according to claim 8, wherein the tape thickness is 5.2 μm or less.

11. 11. The magnetic tape according to claim 8, further comprising a non-magnetic layer containing non-magnetic powder between the non-magnetic support and the magnetic layer.

12. 12. The magnetic tape according to claim 8, wherein the non-magnetic powder in the backcoat layer contains carbon black.

13. 13. The magnetic tape according to claim 8, wherein the perpendicular squareness ratio is 0.60 or more.

14. A magnetic tape cartridge comprising the magnetic tape according to any one of claims 8 to 13 wound around a cartridge reel.

Citation Information

Patent Citations

  • Magnetic tape drive and magnetic tape cartridge

    JP2004355694A

  • Linear tape drive apparatus

    JP2005285268A

  • Magnetic recording medium

    JP2010102818A

  • Magnetic tape and magnetic signal reproduction device

    JP2016212932A

  • Magnetic recording medium

    JP2019003711A