Magnetic tape, magnetic tape cartridge and magnetic tape device

The magnetic tape design with controlled spacing differences on the magnetic layer surface stabilizes the tape's width under tension, addressing head tracking deviations and improving data recording and reproduction accuracy.

JP7575626B2Active Publication Date: 2024-10-29FUJIFILM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2024006552
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-01-19
Publication Date
2024-10-29
Estimated Expiration
2040-01-31

AI Technical Summary

Technical Problem

The challenge of maintaining accurate head tracking on magnetic tapes during recording and reproduction is exacerbated by tension adjustments that can cause the magnetic head to deviate from the target track due to width deformation of the tape, leading to issues like overwriting or reproduction failure.

Method used

A magnetic tape design with a non-magnetic support and a magnetic layer containing ferromagnetic powder, where the spacing difference between specific pressures after cleaning with n-hexane is controlled to 32 nm or less, enhancing the tape's widthwise dimension control through tension adjustment.

Benefits of technology

This design improves the running stability and accuracy of the magnetic tape by minimizing changes in the magnetic head's contact state, reducing friction, and maintaining consistent track alignment, thereby enhancing data integrity and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575626000002
    Figure 0007575626000002
  • Figure 0007575626000003
    Figure 0007575626000003
  • Figure 0007575626000004
    Figure 0007575626000004
Patent Text Reader

Abstract

To provide a magnetic tape that is excellent in running stability when recording and / or reproducing data with a dimension in a width direction of the magnetic tape controlled by adjusting a tension to be applied in a longitudinal direction of the magnetic tape.SOLUTION: One embodiment of the present invention is a magnetic tape in which a differential (S0.1-S1.6) between spacing S0.1 obtained after n-hexane cleaning in a surface of a magnetic layer and spacing S1.6 thereto is equal to or less than 32 nm. S0.1 is a value obtained as the spacing under pressing force of 0.1 atm from a relational expression between pressure and spacing obtained through spacing measurements by respective optical interference methods under pressing force of a plurality of different pressure after the n-hexane cleaning in the surface of the magnetic layer, and S1.6 is the spacing measured by the optical interference method under pressing force of 1.6 atm after the n-hexane cleaning in the surface of the magnetic layer. One embodiment of the present invention is a magnetic tape cartridge and a magnetic tape device that include the magnetic tape.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a magnetic tape, a magnetic tape cartridge, and a magnetic tape device. [Background technology]

[0002] Magnetic recording media include tape-type and disk-type recording media, and tape-type magnetic recording media, that is, magnetic tapes, are primarily used for data storage applications such as data backup and archiving (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6590104 specification Summary of the Invention [Problem to be solved by the invention]

[0004] Data is usually recorded on a magnetic tape by running the magnetic tape in a magnetic tape device (usually called a "drive") and recording data on the data band of the magnetic tape by moving a magnetic head along the data band of the magnetic tape. This forms a data track on the data band. When reproducing the recorded data, the magnetic tape is run in the magnetic tape device and the magnetic head is moved along the data band of the magnetic tape to read the data recorded on the data band.

[0005] In order to improve the accuracy with which the magnetic head tracks the data band of the magnetic tape during the above-described recording and / or reproduction, a system that performs head tracking using a servo signal (hereinafter referred to as a "servo system") has been put into practical use. Furthermore, the width of the magnetic tape is controlled by acquiring width dimensional information of the magnetic tape while it is running using a servo signal, and adjusting the tension applied to the magnetic tape in the longitudinal direction according to the acquired width information (see paragraph 0170 of Patent Document 1 as an example). The above tension adjustment is considered to contribute to suppressing the occurrence of phenomena such as overwriting of recorded data and playback failure, which occur when the magnetic head for recording or playing back data is displaced from the target track position due to width deformation of the magnetic tape during recording or playback. Furthermore, when the magnetic tape is run in a magnetic tape device to record and / or play back data while performing such tension adjustment, high running stability of the magnetic tape is expected to further suppress the occurrence of the above phenomena.

[0006] In view of the above, one aspect of the present invention aims to provide a magnetic tape that has excellent running stability when recording and / or playing back by controlling the width dimension of the magnetic tape by adjusting the tension applied to the magnetic tape in the longitudinal direction. [Means for solving the problem]

[0007] One aspect of the present invention is A non-magnetic support and a magnetic layer containing ferromagnetic powder, The spacing S required on the surface of the magnetic layer after washing with n-hexane 0.1 and spacing S 1.6 Difference from (S 0.1 -S 1.6 ) is 32 nm or less, Above spacing S 0.1 is a value calculated as the spacing under a pressure of 0.1 atm from the relational equation between the pressure and the spacing obtained by measuring the spacing by optical interference method under a plurality of different pressures after cleaning the surface of the magnetic layer with n-hexane, Above spacing S 1.6is the spacing measured by optical interferometry under a pressure of 1.6 atm on the surface of the magnetic layer after washing with n-hexane. Magnetic tape. In the following, the difference (S 0.1 -S 1.6 ) is also referred to simply as "difference". Also, 1 atm = 101325 Pa (pascals).

[0008] In one embodiment, the difference can be 30 nm or less.

[0009] In one embodiment, the difference can be 10 nm or more and 30 nm or less.

[0010] In one embodiment, the magnetic layer can include inorganic oxide particles.

[0011] In one embodiment, the inorganic oxide particles can be composite particles of an inorganic oxide and a polymer.

[0012] In one embodiment, the magnetic tape can have a non-magnetic layer containing non-magnetic powder between the non-magnetic support and the magnetic layer.

[0013] In one embodiment, the magnetic tape can have a backcoat layer containing a nonmagnetic powder on the surface side of the nonmagnetic support opposite to the surface side having the magnetic layer.

[0014] In one embodiment, the magnetic tape may have a tape thickness of 5.3 μm or less.

[0015] One aspect of the present invention relates to a magnetic tape cartridge including the above-mentioned magnetic tape.

[0016] One aspect of the present invention relates to a magnetic tape device including the above-mentioned magnetic tape cartridge. Effect of the Invention

[0017] According to one aspect of the present invention, it is possible to provide a magnetic tape having excellent running stability during recording and / or playback by controlling the widthwise dimension of the magnetic tape by adjusting the tension applied to the magnetic tape in the longitudinal direction. Also, according to one aspect of the present invention, it is possible to provide a magnetic tape cartridge including the magnetic tape and a magnetic tape device including the magnetic tape cartridge. [Brief description of the drawings]

[0018] [Figure 1] 2 shows an example of the arrangement of data bands and servo bands. [Diagram 2] An example of servo pattern arrangement on an LTO (Linear Tape-Open) Ultrium format tape is shown. [Diagram 3] FIG. 1 is a schematic diagram illustrating an example of a magnetic tape device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] [Magnetic tape] One aspect of the present invention is a method for producing a magnetic film having a non-magnetic support and a magnetic layer containing ferromagnetic powder, the method comprising the steps of: 0.1 and spacing S 1.6 Difference from (S 0.1 -S 1.6 ) relates to magnetic tapes with spacings of 32 nm or less. 0.1 is a value calculated as the spacing under a pressure of 0.1 atm from the relationship between the pressure and the spacing obtained by measuring the spacing by optical interference method under a plurality of different pressures after washing the surface of the magnetic layer with n-hexane. 1.6 is the spacing measured by optical interferometry under a pressure of 1.6 atm on the surface of the magnetic layer after washing with n-hexane.

[0020] In the present invention and this specification, "n-hexane cleaning" refers to immersing a sample piece cut out from a magnetic tape in fresh n-hexane (200 g) at a liquid temperature of 20 to 25°C and ultrasonically cleaning (ultrasonic output: 40 kHz) for 100 seconds. A sample piece having a length of 5 cm is cut out from the magnetic tape to be cleaned and subjected to n-hexane cleaning. The width of the magnetic tape and the width of the sample piece cut out from the magnetic tape are usually 1 / 2 inch. For magnetic tapes with a width other than 1 / 2 inch, a sample piece having a length of 5 cm may be cut out and subjected to n-hexane cleaning. The spacing measurement described in detail below is performed after the sample piece after n-hexane cleaning is left in an environment at a temperature of 23°C and a relative humidity of 50% for 24 hours.

[0021] In the present invention and this specification, the "surface of the magnetic layer" of a magnetic tape is synonymous with the surface of the magnetic tape on the magnetic layer side.

[0022] In the present invention and the present specification, "spacing S 0.1 " and "Spacing S 1.6 " is a value calculated by the following method. Spacing S 0.1 In order to obtain the relationship between the pressure and the spacing, the surface of the magnetic layer is subjected to spacing measurement by optical interference method under a plurality of different pressures after n-hexane cleaning, and the relationship between the pressure and the spacing is obtained. More specifically, the relationship is obtained by the following method. The plurality of different pressures are 0.5 atm, 0.6 atm, 0.8 atm, 1.0 atm, 1.3 atm, and 1.6 atm. A magnetic tape (more specifically, the above sample piece; the same applies below) and a transparent plate-like member (e.g., a glass plate, etc.) are superimposed so that the magnetic layer surface of the magnetic tape faces the transparent plate-like member, and a pressing member is pressed from the side opposite the magnetic layer side of the magnetic tape with a pressure of 0.5 atm. In this state, light is irradiated onto the magnetic layer surface of the magnetic tape through the transparent plate-like member (irradiation area: 150,000 to 200,000 μm 2), the spacing (distance) between the magnetic layer surface of the magnetic tape and the magnetic tape side surface of the transparent plate-like member is determined based on the intensity of the interference light (for example, the contrast of the interference fringe image) generated by the optical path difference between the reflected light from the magnetic layer surface of the magnetic tape and the reflected light from the magnetic tape side surface of the transparent plate-like member. The light irradiated here is not particularly limited. In the case where the irradiated light has an emission wavelength over a relatively wide wavelength range, such as white light containing light of multiple wavelengths, a member having a function of selectively cutting light of a specific wavelength or light other than a specific wavelength range, such as an interference filter, is disposed between the transparent plate-like member and the light receiving unit that receives the reflected light, and light of a part of the wavelengths or light of a part of the wavelength range of the reflected light is selectively made to enter the light receiving unit. In the case where the irradiated light is light having a single emission peak (so-called monochromatic light), the above member does not need to be used. The wavelength of the light incident on the light receiving unit can be, for example, in the range of 500 to 700 nm. However, the wavelength of the light incident on the light receiving unit is not limited to the above range. The transparent plate-like member may be any member having transparency that allows the light to pass through it to such an extent that interference light can be obtained by irradiating the magnetic tape with light through the member. The interference fringe image obtained by the above spacing measurement is divided into 300,000 points, and the spacing at each point (the distance between the magnetic layer surface of the magnetic tape and the magnetic tape side surface of the transparent plate-like member) is determined and plotted as a histogram. The most frequent value in this histogram is taken as the spacing measured under a pressure of 0.5 atm. Five sample pieces are cut out from the same magnetic tape, and for each sample piece, after washing with n-hexane, a pressure member is pressed against the sample piece at a pressure of 0.5 atm to determine the spacing. The pressure is then increased to 0.6 atm, 0.8 atm, 1.0 atm, 1.3 atm, and 1.6 atm, and the spacing measured under each pressure is determined by the above method. The spacing value thus obtained under each pressure was plotted against the pressure at the time of pressure application, and the following formula 1 was calculated: (Formula 1) h=c1p c2 In Equation 1, h is the average spacing, p is the pressure at the time of pressing, c1 and c2 are fitting parameters, and C1 and C2 are found by fitting. Using the C1 and C2 thus obtained, the relation between pressure and spacing is derived. That is, the spacing under pressure p is expressed as S p Then, the relation is "S p =C1(p) C2 Therefore, the spacing S under pressure of 0.1 atm is 0.1 is expressed as follows: (Formula 2) S 0.1 =C1(0.1) C2 In this way, the relationship was derived for each of the five test pieces, and S was calculated using the derived relationship. 0.1 The S calculated for each of the five sample pieces is 0.1 The arithmetic mean of the magnetic tape to be measured is 0.1 Let us assume that. Spacing S 1.6 For the above, the arithmetic average of the spacing measurements obtained for five sample pieces under a pressure of 1.6 atm was used as the S of the magnetic tape being measured. 1.6 Let us assume that. And the S obtained in this way 0.1 and S. 1.6 The difference between the measured magnetic tape (S 0.1 -S 1.6 ) is required. The above spacing measurements can be performed using a commercially available tape spacing analyzer (TSA) such as the Tape Spacing Analyzer manufactured by Micro Physics Corp. The spacing measurements in the examples were performed using the Tape Spacing Analyzer manufactured by Micro Physics Corp.

[0023] In the above magnetic tape, the difference (S 0.1 -S 1.6 ) is 32 nm or less. The inventors speculate that this can contribute to improving the running stability (hereinafter also simply referred to as "running stability") when recording and / or reproducing by controlling the width direction dimension of the magnetic tape by adjusting the tension applied in the longitudinal direction of the magnetic tape. The details are as follows. In a magnetic tape device that controls the width of the magnetic tape by adjusting the tension applied in the longitudinal direction of the magnetic tape, the greater the tension applied in the longitudinal direction of the magnetic tape, the greater the shrinkage of the width of the magnetic tape (i.e., the narrower it can be), and the smaller the tension, the smaller the degree of shrinkage. In this way, the width of the magnetic tape can be controlled by adjusting the tension applied in the longitudinal direction of the magnetic tape. On the other hand, recording of data on a magnetic tape and reproduction of the recorded data are usually performed by contacting and sliding the magnetic head against the magnetic layer surface of the magnetic tape. When the above-mentioned tension adjustment is performed, the tension applied in the longitudinal direction of the magnetic tape may vary. This may cause the contact state between the magnetic head and the magnetic tape running in the magnetic tape device to vary, and therefore the pressure applied to the magnetic layer surface by contact with the magnetic head may also vary. The magnetic layer surface usually has protrusions, and these protrusions can contribute to lowering the coefficient of friction when the magnetic layer surface and the magnetic head slide by reducing the portion where the magnetic layer surface contacts the magnetic head (so-called true contact). However, if the height of such protrusions changes significantly due to changes in the pressure applied to the magnetic layer surface, the contact state between the magnetic layer surface and the magnetic head will change significantly. It is believed that if such a large change can be suppressed, the running stability can be improved. In this regard, the S obtained by the above method 0.1 and S. 1.6 Difference from (S 0.1 -S 1.6The fact that the protrusion height is as small as 32 nm or less is presumably due to the fact that the height of the protrusions on the magnetic layer surface is unlikely to change significantly even if the pressure applied to the magnetic layer surface changes. The inventors presume that this leads to improved running stability. However, the present invention is not limited to the above speculation. 0.1 and spacing S 1.6 Regarding the pressure, in the present invention, 0.1 atm and 1.6 atm are adopted as exemplary values ​​of pressure, and the pressure applied to the magnetic layer surface of the magnetic tape during sliding with the magnetic head is not limited to the above pressure. It has been newly discovered as a result of the inventor's earnest research that by controlling the above difference obtained by adopting the above pressure, it is possible to improve the running stability during recording and / or reproduction by adjusting the tension applied in the longitudinal direction of the magnetic tape and thereby controlling the dimension in the width direction of the magnetic tape.

[0024] The above magnetic tape will now be described in more detail.

[0025] <Magnetic layer> (Difference(S 0.1 -S 1.6 )) Difference between the above magnetic tapes (S 0.1 -S 1.6) is 32 nm or less, and from the viewpoint of further improving running stability, it is preferably 31 nm or less, more preferably 30 nm or less, even more preferably 29 nm or less, even more preferably 28 nm or less, even more preferably 27 nm or less, even more preferably 26 nm or less, even more preferably 25 nm or less, even more preferably 24 nm or less, even more preferably 23 nm or less, and even more preferably 22 nm or less. The difference can be, for example, more than 0 nm, 1 nm or more, 3 nm or more, 5 nm or more, or 10 nm or more. The smaller the difference, the more preferable it is from the viewpoint of improving running stability. The difference can be controlled by the type of non-magnetic filler (hereinafter referred to as "protrusion forming agent") that can form protrusions on the magnetic layer surface and the manufacturing conditions of the magnetic tape. This point will be described in detail later.

[0026] S of the above magnetic tape 0.1 and S 1.6 is the difference (S 0.1 -S 1.6 ) is not particularly limited as long as it is 32 nm or less. On the other hand, from the viewpoint of improving electromagnetic conversion characteristics, S 0.1 is preferably 70 nm or less, more preferably 60 nm or less, even more preferably 50 nm or less, and even more preferably 40 nm or less. In addition, from the viewpoint of keeping the coefficient of friction low mainly at the initial stage of sliding with the magnetic head, S 0.1 is preferably 10 nm or more, more preferably 15 nm or more, even more preferably 20 nm or more, and even more preferably 25 nm or more. 1.6 is preferably 1 nm or more, more preferably 3 nm or more, even more preferably 5 nm or more, and even more preferably 7 nm or more. 1.6 can be, for example, 30 nm or less, 25 nm or less, 20 nm or less, or 15 nm or less.

[0027] (Ferromagnetic powder) As the ferromagnetic powder contained in the magnetic layer, one or more of the ferromagnetic powders known as ferromagnetic powders used in the magnetic layers of various magnetic recording media can be used in combination. It is preferable to use a ferromagnetic powder with a small average particle size from the viewpoint of improving recording density. From this viewpoint, the average particle size of the ferromagnetic powder is preferably 50 nm or less, more preferably 45 nm or less, even more preferably 40 nm or less, even more preferably 35 nm or less, even more preferably 30 nm or less, even more preferably 25 nm or less, and even more preferably 20 nm or less. On the other hand, from the viewpoint of magnetization stability, the average particle size of the ferromagnetic powder is preferably 5 nm or more, more preferably 8 nm or more, even more preferably 10 nm or more, even more preferably 15 nm or more, and even more preferably 20 nm or more.

[0028] Hexagonal Ferrite Powder A preferred specific example of the ferromagnetic powder is hexagonal ferrite powder. For details of the hexagonal ferrite powder, see, for example, JP2011-225417A, paragraphs 0012-0030, JP2011-216149A, paragraphs 0134-0136, JP2012-204726A, paragraphs 0013-0030, and JP2015-127985A, paragraphs 0029-0084.

[0029] In the present invention and this specification, the term "hexagonal ferrite powder" refers to a ferromagnetic powder in which a hexagonal ferrite type crystal structure is detected as the main phase by X-ray diffraction analysis. The main phase refers to a structure to which the most intense diffraction peak belongs in the X-ray diffraction spectrum obtained by X-ray diffraction analysis. For example, when the most intense diffraction peak in the X-ray diffraction spectrum obtained by X-ray diffraction analysis is assigned to a hexagonal ferrite type crystal structure, it is determined that the hexagonal ferrite type crystal structure has been detected as the main phase. When only a single structure is detected by X-ray diffraction analysis, the detected structure is regarded as the main phase. The hexagonal ferrite type crystal structure contains at least an iron atom, a divalent metal atom, and an oxygen atom as constituent atoms. The divalent metal atom is a metal atom that can become a divalent cation as an ion, and examples of such include alkaline earth metal atoms such as strontium atoms, barium atoms, and calcium atoms, and lead atoms. In the present invention and this specification, the hexagonal strontium ferrite powder refers to a powder in which the main divalent metal atom contained therein is a strontium atom, and the hexagonal barium ferrite powder refers to a powder in which the main divalent metal atom contained therein is a barium atom. The main divalent metal atom refers to the divalent metal atom that is the most abundant of the divalent metal atoms contained in the powder on an atomic % basis. However, the above divalent metal atoms do not include rare earth atoms. In the present invention and this specification, the "rare earth atom" is selected from the group consisting of scandium atoms (Sc), yttrium atoms (Y), and lanthanoid atoms. The lanthanide atom is selected from the group consisting of a lanthanum atom (La), a cerium atom (Ce), a praseodymium atom (Pr), a neodymium atom (Nd), a promethium atom (Pm), a samarium atom (Sm), a europium atom (Eu), a gadolinium atom (Gd), a terbium atom (Tb), a dysprosium atom (Dy), a holmium atom (Ho), an erbium atom (Er), a thulium atom (Tm), a ytterbium atom (Yb), and a lutetium atom (Lu).

[0030] Hereinafter, the hexagonal strontium ferrite powder, which is one embodiment of the hexagonal ferrite powder, will be described in further detail.

[0031] The activation volume of the hexagonal strontium ferrite powder is preferably 800 to 1600 nm 3 The finely divided hexagonal strontium ferrite powder having an activation volume in the above range is suitable for producing a magnetic tape exhibiting excellent electromagnetic conversion characteristics. The activation volume of the hexagonal strontium ferrite powder is preferably 800 nm 3 For example, 850 nm or more. 3 From the viewpoint of further improving the electromagnetic conversion characteristics, the activation volume of the hexagonal strontium ferrite powder can be 1500 nm or more. 3 More preferably, it is 1400 nm or less. 3 More preferably, it is 1300 nm or less. 3 More preferably, it is 1200 nm or less. 3 More preferably, it is equal to or less than 1100 nm. 3 It is even more preferable that the activation volume of the hexagonal barium ferrite powder is equal to or less than 1000 nm. The same is true for the activation volume of the hexagonal barium ferrite powder.

[0032] "Activation volume" is a unit of magnetization reversal and is an index showing the magnetic size of a particle. The activation volume and the anisotropy constant Ku described in the present invention and this specification are values ​​obtained by measuring the coercive force Hc measurement section at magnetic field sweep speeds of 3 minutes and 30 minutes (measurement temperature: 23°C ± 1°C) using a vibrating sample magnetometer, and calculating from the following relationship between Hc and activation volume V. The unit of the anisotropy constant Ku is 1 erg / cc = 1.0 x 10 -1 J / m 3 It is. Hc=2Ku / Ms{1-[(kT / KuV)ln(At / 0.693)] 1 / 2} [In the above formula, Ku: anisotropy constant (unit: J / m 3 ), Ms: saturation magnetization (unit: kA / m), k: Boltzmann constant, T: absolute temperature (unit: K), V: activation volume (unit: cm 3), A: spin precession frequency (unit: s -1 ), t: magnetic field reversal time (unit: s)]

[0033] The anisotropy constant Ku can be used as an index of reduction in thermal fluctuation, in other words, improvement in thermal stability. The hexagonal strontium ferrite powder is preferably 1.8×10 5 J / m 3 More preferably, the Ku is 2.0×10 or more. 5 J / m 3 The Ku of the hexagonal strontium ferrite powder can be, for example, 2.5×10 5 J / m 3 However, since a higher Ku value means higher thermal stability and is preferable, the Ku value is not limited to the above-mentioned values.

[0034] The hexagonal strontium ferrite powder may or may not contain rare earth atoms. When the hexagonal strontium ferrite powder contains rare earth atoms, it is preferable that the rare earth atoms are contained at a content (bulk content) of 0.5 to 5.0 atomic % relative to 100 atomic % of iron atoms. In one embodiment, the hexagonal strontium ferrite powder containing rare earth atoms can have uneven distribution of rare earth atoms in the surface layer portion. In the present invention and this specification, the term "surface distribution of rare earth atoms" refers to the rare earth atom content relative to 100 atomic % of iron atoms in a solution obtained by partially dissolving a hexagonal strontium ferrite powder in an acid (hereinafter referred to as "surface content of rare earth atoms" or simply "surface content" for rare earth atoms), which is greater than the rare earth atom content relative to 100 atomic % of iron atoms in a solution obtained by completely dissolving a hexagonal strontium ferrite powder in an acid (hereinafter referred to as "bulk content of rare earth atoms" or simply "bulk content" for rare earth atoms), Rare earth atom surface content / rare earth atom bulk content>1.0 The rare earth atom content of the hexagonal strontium ferrite powder described later is synonymous with the rare earth atom bulk content. In contrast, partial dissolution using an acid dissolves the surface layer of the particles constituting the hexagonal strontium ferrite powder, so the rare earth atom content in the solution obtained by partial dissolution is the rare earth atom content in the surface layer of the particles constituting the hexagonal strontium ferrite powder. The rare earth atom surface layer content satisfying the ratio of "rare earth atom surface layer content / rare earth atom bulk content>1.0" means that the rare earth atoms are unevenly distributed (i.e., more present in the surface layer) in the particles constituting the hexagonal strontium ferrite powder. In the present invention and this specification, the surface layer refers to a portion of the region extending from the surface of the particles constituting the hexagonal strontium ferrite powder toward the inside.

[0035] When the hexagonal strontium ferrite powder contains rare earth atoms, the rare earth atom content (bulk content) is preferably in the range of 0.5 to 5.0 atomic % relative to 100 atomic % of iron atoms. It is considered that the rare earth atoms contained in the bulk content in the above range and the rare earth atoms unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder contribute to suppressing the decrease in the reproduction output during repeated reproduction. This is presumed to be because the hexagonal strontium ferrite powder contains rare earth atoms in the bulk content in the above range and the rare earth atoms unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder can increase the anisotropy constant Ku. The higher the value of the anisotropy constant Ku, the more the occurrence of a phenomenon called thermal fluctuation can be suppressed (in other words, the thermal stability can be improved). By suppressing the occurrence of thermal fluctuation, the decrease in the reproduction output during repeated reproduction can be suppressed. It is speculated that the uneven distribution of rare earth atoms in the surface layer of hexagonal strontium ferrite powder particles contributes to stabilizing the spin of the iron (Fe) sites in the crystal lattice of the surface layer, thereby increasing the anisotropy constant Ku. In addition, it is presumed that using the hexagonal strontium ferrite powder having rare earth atom uneven distribution on the surface as the ferromagnetic powder of the magnetic layer also contributes to suppressing the wear of the magnetic layer surface due to sliding with the magnetic head. That is, it is presumed that the hexagonal strontium ferrite powder having rare earth atom uneven distribution on the surface can also contribute to improving the running durability of the magnetic tape. This is presumed to be because the uneven distribution of rare earth atoms on the surface of the particles constituting the hexagonal strontium ferrite powder contributes to improving the interaction between the particle surface and the organic substance (e.g., binder and / or additive) contained in the magnetic layer, and as a result, the strength of the magnetic layer is improved. From the viewpoint of further suppressing the decrease in regeneration output during repeated regeneration and / or further improving running durability, the rare earth atom content (bulk content) is more preferably in the range of 0.5 to 4.5 atomic %, even more preferably in the range of 1.0 to 4.5 atomic %, and even more preferably in the range of 1.5 to 4.5 atomic %.

[0036] The bulk content is the content obtained by completely dissolving the hexagonal strontium ferrite powder. In the present invention and this specification, unless otherwise specified, the content of an atom refers to the bulk content obtained by completely dissolving the hexagonal strontium ferrite powder. The hexagonal strontium ferrite powder containing rare earth atoms may contain only one rare earth atom as a rare earth atom, or may contain two or more rare earth atoms. The bulk content when containing two or more rare earth atoms is obtained for the total of two or more rare earth atoms. This point is the same for other components in the present invention and this specification. That is, unless otherwise specified, a certain component may be used in only one type or in two or more types. When two or more types are used, the content or content refers to the total of two or more types.

[0037] When the hexagonal strontium ferrite powder contains rare earth atoms, the rare earth atoms contained therein may be any one or more of rare earth atoms. From the viewpoint of further suppressing the decrease in the reproduction output during repeated reproduction, preferred rare earth atoms include neodymium atoms, samarium atoms, yttrium atoms and dysprosium atoms, more preferred are neodymium atoms, samarium atoms and yttrium atoms, and even more preferred are neodymium atoms.

[0038] In the hexagonal strontium ferrite powder having rare earth atom uneven distribution in the surface layer, the rare earth atoms may be unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder, and the degree of uneven distribution is not limited. For example, for the hexagonal strontium ferrite powder having rare earth atom uneven distribution in the surface layer, the ratio of the surface content of rare earth atoms obtained by partial dissolution under the dissolution conditions described below to the bulk content of rare earth atoms obtained by complete dissolution under the dissolution conditions described below, "surface content / bulk content", is more than 1.0 and can be 1.5 or more. The "surface content / bulk content" being greater than 1.0 means that the rare earth atoms are unevenly distributed in the surface layer (i.e., more than in the interior) in the particles constituting the hexagonal strontium ferrite powder. In addition, the ratio of the surface layer content of rare earth atoms obtained by partial dissolution under the dissolution conditions described later to the bulk content of rare earth atoms obtained by total dissolution under the dissolution conditions described later, "surface layer content / bulk content", can be, for example, 10.0 or less, 9.0 or less, 8.0 or less, 7.0 or less, 6.0 or less, 5.0 or less, or 4.0 or less. However, in a hexagonal strontium ferrite powder having rare earth atom surface layer uneven distribution, it is sufficient that the rare earth atoms are unevenly distributed in the surface layer of the particles constituting the hexagonal strontium ferrite powder, and the above "surface layer content / bulk content" is not limited to the upper or lower limit exemplified.

[0039] The partial and total dissolution of hexagonal strontium ferrite powder will be described below. For hexagonal strontium ferrite powder present as powder, the sample powders to be partially and completely dissolved are taken from the same lot of powder. On the other hand, for hexagonal strontium ferrite powder contained in the magnetic layer of a magnetic tape, a part of the hexagonal strontium ferrite powder taken out from the magnetic layer is subjected to partial dissolution, and the other part is subjected to total dissolution. The hexagonal strontium ferrite powder can be taken out from the magnetic layer by, for example, the method described in paragraph 0032 of JP 2015-91747 A. The above-mentioned partial dissolution means that the hexagonal strontium ferrite powder is dissolved to such an extent that the remaining powder can be visually confirmed in the liquid at the end of dissolution. For example, the partial dissolution can dissolve a region of 10 to 20 mass% of the particles constituting the hexagonal strontium ferrite powder, with the whole particles being 100 mass%. On the other hand, the above-mentioned complete dissolution means that the hexagonal strontium ferrite powder is dissolved to such an extent that the remaining powder cannot be visually confirmed in the liquid at the end of dissolution. The partial dissolution and the surface layer content are measured, for example, by the following method. Note that the dissolution conditions such as the amount of sample powder are merely examples, and any dissolution conditions that allow partial or complete dissolution can be used. A container (e.g., a beaker) containing 12 mg of sample powder and 10 mL of 1 mol / L hydrochloric acid is placed on a hot plate set at 70°C for 1 hour. The resulting solution is filtered through a 0.1 μm membrane filter. Elemental analysis of the filtrate thus obtained is performed using an inductively coupled plasma (ICP) analyzer. In this way, the surface layer content of rare earth atoms relative to 100 atomic % of iron atoms can be determined. When multiple types of rare earth atoms are detected by elemental analysis, the total content of all rare earth atoms is taken as the surface layer content. This is also true for the measurement of bulk content. On the other hand, the total dissolved and bulk contents are measured, for example, by the following method. A container (e.g., a beaker) containing 12 mg of sample powder and 10 mL of 4 mol / L hydrochloric acid is placed on a hot plate set at 80° C. for 3 hours. After that, the bulk content relative to 100 atomic % of iron atoms can be calculated by carrying out the same procedure as the partial dissolution and surface layer content measurement described above.

[0040] From the viewpoint of increasing the reproduction output when reproducing data recorded on a magnetic tape, it is desirable that the mass magnetization σs of the ferromagnetic powder contained in the magnetic tape is high. In this regard, hexagonal strontium ferrite powder containing rare earth atoms but not having uneven distribution of rare earth atoms in the surface layer has a tendency to have a significantly lower σs than hexagonal strontium ferrite powder not containing rare earth atoms. In contrast, hexagonal strontium ferrite powder having uneven distribution of rare earth atoms in the surface layer is considered to be preferable in terms of suppressing such a large decrease in σs. In one embodiment, the σs of the hexagonal strontium ferrite powder is 45 A·m 2 / kg or more, and 47A·m 2 / kg or more. On the other hand, from the viewpoint of noise reduction, σs is 80A·m 2 / kg or less, and 60A·m 2 / kg or less. σs can be measured using a known measuring device capable of measuring magnetic properties, such as a vibrating sample magnetometer. In the present invention and this specification, unless otherwise specified, the mass magnetization σs is a value measured at a magnetic field strength of 15 kOe. 1 [kOe]=10 6 / 4π[A / m].

[0041] Regarding the content (bulk content) of the constituent atoms of the hexagonal strontium ferrite powder, the strontium atom content can be, for example, in the range of 2.0 to 15.0 atomic % relative to 100 atomic % of iron atoms. In one embodiment, the divalent metal atoms contained in the hexagonal strontium ferrite powder can be only strontium atoms. In another embodiment, the hexagonal strontium ferrite powder can also contain one or more other divalent metal atoms in addition to strontium atoms. For example, it can contain barium atoms and / or calcium atoms. When divalent metal atoms other than strontium atoms are contained, the barium atom content and calcium atom content in the hexagonal strontium ferrite powder can each be, for example, in the range of 0.05 to 5.0 atomic % relative to 100 atomic % of iron atoms.

[0042] Known crystal structures of hexagonal ferrite include magnetoplumbite type (also called "M type"), W type, Y type, and Z type. The hexagonal strontium ferrite powder may have any of the crystal structures. The crystal structure can be confirmed by X-ray diffraction analysis. The hexagonal strontium ferrite powder may be one in which a single crystal structure or two or more types of crystal structures are detected by X-ray diffraction analysis. For example, in one embodiment, the hexagonal strontium ferrite powder may be one in which only the M-type crystal structure is detected by X-ray diffraction analysis. For example, the M-type hexagonal ferrite is AFe 12 O 19Here, A represents a divalent metal atom, and when the hexagonal strontium ferrite powder is of the M type, A is only a strontium atom (Sr), or when A contains a plurality of divalent metal atoms, the strontium atom (Sr) accounts for the largest proportion on an atomic % basis as described above. The divalent metal atom content of the hexagonal strontium ferrite powder is usually determined by the type of crystal structure of the hexagonal ferrite, and is not particularly limited. The same applies to the iron atom content and the oxygen atom content. The hexagonal strontium ferrite powder contains at least an iron atom, a strontium atom, and an oxygen atom, and may further contain a rare earth atom. Furthermore, the hexagonal strontium ferrite powder may or may not contain atoms other than these atoms. As an example, the hexagonal strontium ferrite powder may contain an aluminum atom (Al). The content of aluminum atoms can be, for example, 0.5 to 10.0 atomic % relative to 100 atomic % of iron atoms. From the viewpoint of further suppressing the decrease in the reproduction output during repeated reproduction, the hexagonal strontium ferrite powder contains iron atoms, strontium atoms, oxygen atoms, and rare earth atoms, and the content of atoms other than these atoms is preferably 10.0 atomic % or less, more preferably in the range of 0 to 5.0 atomic %, relative to 100 atomic % of iron atoms, and may be 0 atomic %. That is, in one embodiment, the hexagonal strontium ferrite powder may not contain atoms other than iron atoms, strontium atoms, oxygen atoms, and rare earth atoms. The content expressed in atomic % above is obtained by converting the content (unit: mass %) of each atom obtained by completely dissolving the hexagonal strontium ferrite powder into a value expressed in atomic % using the atomic weight of each atom. In addition, in the present invention and this specification, "not containing" a certain atom means that the content measured by an ICP analyzer after completely dissolving is 0 mass %. The detection limit of an ICP analyzer is usually 0.01 ppm (parts per million) or less on a mass basis. The above term "free" is used to mean that the content is below the detection limit of the ICP analyzer.In one embodiment, the hexagonal strontium ferrite powder may be free of bismuth atoms (Bi).

[0043] metal powder A specific preferred example of the ferromagnetic powder is a ferromagnetic metal powder. For details of the ferromagnetic metal powder, reference can be made to, for example, paragraphs 0137 to 0141 of JP 2011-216149 A and paragraphs 0009 to 0023 of JP 2005-251351 A.

[0044] ε-iron oxide powder A preferred specific example of the ferromagnetic powder is ε-iron oxide powder. In the present invention and this specification, the term "ε-iron oxide powder" refers to a ferromagnetic powder in which an ε-iron oxide type crystal structure is detected as the main phase by X-ray diffraction analysis. For example, when the highest intensity diffraction peak in the X-ray diffraction spectrum obtained by X-ray diffraction analysis is attributed to an ε-iron oxide type crystal structure, it is determined that the ε-iron oxide type crystal structure is detected as the main phase. Known methods for producing ε-iron oxide powder include a method of producing it from goethite and a reverse micelle method. All of the above production methods are publicly known. In addition, for a method for producing ε-iron oxide powder in which a part of Fe is replaced by a substitution atom such as Ga, Co, Ti, Al, or Rh, reference can be made to, for example, J. Jpn. Soc. Powder Metallurgy Vol. 61 Supplement, No. S1, pp. S280-S284, J. Mater. Chem. C, 2013, 1, pp.5200-5206, etc. However, the method for producing the ε-iron oxide powder that can be used as the ferromagnetic powder in the magnetic layer of the magnetic tape is not limited to the method given here.

[0045] The activation volume of the ε-iron oxide powder is preferably 300 to 1500 nm 3 The finely divided ε-iron oxide powder exhibiting an activation volume in the above range is suitable for producing a magnetic tape exhibiting excellent electromagnetic conversion characteristics. The activation volume of the ε-iron oxide powder is preferably 300 nm 3For example, 500 nm or more. 3 From the viewpoint of further improving the electromagnetic conversion characteristics, the activation volume of the ε-iron oxide powder can be 1400 nm or more. 3 More preferably, it is 1300 nm or less. 3 More preferably, it is 1200 nm or less. 3 More preferably, it is equal to or less than 1100 nm. 3 It is even more preferred that:

[0046] The anisotropy constant Ku can be used as an index of the reduction in thermal fluctuation, in other words, the improvement in thermal stability. The ε-iron oxide powder is preferably 3.0×10 4 J / m 3 More preferably, the Ku is 8.0×10 or more. 4 J / m 3 The Ku of the ε-iron oxide powder can be, for example, 3.0×10 5 J / m 3 However, since a higher Ku value means higher thermal stability and is preferable, the Ku value is not limited to the above-mentioned values.

[0047] From the viewpoint of increasing the reproduction output when reproducing data recorded on a magnetic tape, it is desirable that the mass magnetization σs of the ferromagnetic powder contained in the magnetic tape is high. In this regard, in one embodiment, the σs of the ε-iron oxide powder is 8 A m 2 / kg or more, and can be 12 A m 2 On the other hand, the σs of ε-iron oxide powder is 40 A m 2 / kg or less, and 35A·m 2 It is more preferable that the amount is not more than 1 / kg.

[0048] In the present invention and this specification, unless otherwise specified, the average particle size of various powders such as ferromagnetic powders is a value measured by the following method using a transmission electron microscope. The powder is photographed at a magnification of 100,000 times using a transmission electron microscope, and then printed on photographic paper at a total magnification of 500,000 times to obtain a photograph of the particles that make up the powder. From the obtained particle photograph, the target particle is selected, the particle's outline is traced with a digitizer, and the particle (primary particle) size is measured. Primary particles are independent particles that are not aggregated. The above measurements are carried out for 500 randomly selected particles. The arithmetic mean of the particle sizes of the 500 particles thus obtained is the average particle size of the powder. As the transmission electron microscope, for example, a Hitachi transmission electron microscope H-9000 type can be used. The particle size can be measured using a known image analysis software, for example, Carl Zeiss image analysis software KS-400. The average particle size shown in the examples described below is a value measured using a Hitachi transmission electron microscope H-9000 type as the transmission electron microscope and Carl Zeiss image analysis software KS-400 as the image analysis software, unless otherwise specified. In the present invention and this specification, powder means a collection of multiple particles. For example, ferromagnetic powder means a collection of multiple ferromagnetic particles. In addition, the collection of multiple particles is not limited to a form in which the particles constituting the collection are in direct contact with each other, and also includes a form in which a binder, additive, etc., described later, are interposed between the particles. The term particle is sometimes used to refer to powder.

[0049] As a method for collecting sample powder from the magnetic tape for particle size measurement, for example, the method described in paragraph 0015 of JP 2011-048878 A can be used.

[0050] In the present invention and this specification, unless otherwise specified, the size of the particles constituting the powder (particle size) is determined by the shape of the particles observed in the particle photograph. (1) In the case of needle-shaped, spindle-shaped, columnar (where the height is greater than the maximum major axis of the base), etc., it is expressed by the length of the major axis that constitutes the particle, i.e., the major axis length. (2) In the case of a plate or columnar shape (where the thickness or height is smaller than the maximum long diameter of the plate or base), it shall be expressed by the maximum long diameter of the plate or base. (3) In the case of a particle having a spherical, polyhedral, or unspecified shape, and the major axis of the particle cannot be specified from its shape, the particle is expressed as the equivalent circle diameter, which is determined by the circle projection method.

[0051] The average acicular ratio of a powder refers to the arithmetic average of the short axis length of the particles, i.e., the short axis length, the (long axis length / short axis length) value of each particle, and the values ​​obtained for the 500 particles. Here, unless otherwise specified, the short axis length refers to the length of the short axis constituting the particle in the above definition of particle size (1), and to the thickness or height in the above definition of particle size (2), and in the above definition of particle size (3), since there is no distinction between the long axis and the short axis, (long axis length / short axis length) is considered to be 1 for the sake of convenience. Unless otherwise specified, when the particle shape is specific, for example, in the case of the above definition of particle size (1), the average particle size is the average major axis length, in the case of definition (2), the average particle size is the average plate diameter, and in the case of definition (3), the average particle size is the average diameter (also called the average particle diameter or average particle size).

[0052] The content (filling rate) of the ferromagnetic powder in the magnetic layer is preferably in the range of 50 to 90 mass %, and more preferably in the range of 60 to 90 mass %. A high filling rate of the ferromagnetic powder in the magnetic layer is preferable from the viewpoint of improving recording density.

[0053] (Binding Agent) The magnetic tape may be a coated magnetic tape, and may contain a binder in the magnetic layer. The binder is one or more kinds of resin. As the binder, various resins that are usually used as binders for coated magnetic recording media may be used. For example, as the binder, a resin selected from polyurethane resin, polyester resin, polyamide resin, vinyl chloride resin, acrylic resin copolymerized with styrene, acrylonitrile, methyl methacrylate, etc., cellulose resin such as nitrocellulose, epoxy resin, phenoxy resin, polyvinyl acetal, polyvinyl butyral, etc. may be used alone or in combination of a plurality of resins. Among these, polyurethane resin, acrylic resin, cellulose resin, and vinyl chloride resin are preferred. These resins may be homopolymers or copolymers. These resins may also be used as binders in the nonmagnetic layer and / or backcoat layer described later. For the above binders, refer to paragraphs 0028 to 0031 of JP-A-2010-24113. The binder may also be a radiation curable resin such as an electron beam curable resin. For information on radiation curable resins, see paragraphs 0044 to 0045 of JP2011-048878A. The average molecular weight of the resin used as the binder can be, for example, 10,000 or more and 200,000 or less in weight average molecular weight. The weight average molecular weight in the present invention and this specification is a value obtained by converting a value measured under the following measurement conditions by gel permeation chromatography (GPC) into polystyrene equivalent. The weight average molecular weight of the binder shown in the examples described later is a value obtained by converting a value measured under the following measurement conditions into polystyrene equivalent. The binder can be used in an amount of, for example, 1.0 to 30.0 parts by mass per 100.0 parts by mass of the ferromagnetic powder. GPC equipment: HLC-8120 (Tosoh Corporation) Column: TSK gel Multipore HXL-M (Tosoh Corporation, 7.8 mm ID(Inner Diameter)×30.0cm) Eluent: tetrahydrofuran (THF)

[0054] (hardening agent) A curing agent can also be used together with the binder. In one embodiment, the curing agent can be a thermosetting compound that undergoes a curing reaction (crosslinking reaction) by heating, and in another embodiment, it can be a photocuring compound that undergoes a curing reaction (crosslinking reaction) by irradiation with light. As the curing reaction progresses during the manufacturing process of the magnetic tape, at least a part of the curing agent can be contained in the magnetic layer in a state of reacting (crosslinking) with other components such as the binder. A preferred curing agent is a thermosetting compound, and polyisocyanate is suitable. For details on polyisocyanate, refer to paragraphs 0124 to 0125 of JP-A-2011-216149. The curing agent can be used in an amount of, for example, 0 to 80.0 parts by mass relative to 100.0 parts by mass of the binder in the magnetic layer-forming composition, and preferably 50.0 to 80.0 parts by mass from the viewpoint of improving the strength of each layer such as the magnetic layer.

[0055] (Other Ingredients) The magnetic layer may contain one or more additives as necessary. The additives may be selected from commercially available products according to the desired properties. Alternatively, compounds synthesized by known methods may be used as additives. An example of the additive is the above-mentioned curing agent. In addition, additives that may be contained in the magnetic layer include non-magnetic fillers, lubricants, dispersants, dispersion aids, antifungal agents, antistatic agents, antioxidants, etc. Non-magnetic fillers are synonymous with non-magnetic particles or non-magnetic powders. Examples of non-magnetic fillers include protrusion-forming agents and non-magnetic fillers that can function as abrasives (hereinafter referred to as "abrasives"). In addition, known additives such as various polymers described in paragraphs 0030 to 0080 of JP2016-051493A may also be used as additives.

[0056] As the protrusion-forming agent, which is one form of non-magnetic filler, particles of inorganic substances can be used, particles of organic substances can be used, and composite particles of inorganic substances and organic substances can be used. Examples of inorganic substances include inorganic oxides such as metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, metal sulfides, etc., and inorganic oxides are preferred. In one embodiment, the protrusion-forming agent can be inorganic oxide-based particles. Here, "based" is used to mean "including." One embodiment of inorganic oxide-based particles is a particle made of an inorganic oxide. Another embodiment of inorganic oxide-based particles is a composite particle of an inorganic oxide and an organic substance, and a specific example is a composite particle of an inorganic oxide and a polymer. Examples of such particles include, for example, particles in which a polymer is bonded to the surface of an inorganic oxide particle.

[0057] The above S 0.1 can be controlled mainly by the particle size of the protrusion-forming agent. The average particle size of the protrusion-forming agent can be, for example, 30 to 300 nm, and preferably 40 to 200 nm. Also, depending on the manufacturing conditions of the magnetic tape, mainly S 0.1 On the other hand, S 1.6 The protrusion-forming agent can be controlled by its particle size as well as its shape. The closer the particle shape is to a perfect sphere, the smaller the resistance to indentation when a large pressure is applied, and the easier it is to be pressed into the magnetic layer, resulting in the S 1.6 On the other hand, if the particle shape is not spherical, for example, if it has a shape that is called an irregular shape, it is likely to have a large resistance to being pressed into the magnetic layer when a large pressure is applied, and the S 1.6 In addition, particles with an inhomogeneous surface and low surface smoothness tend to have a large indentation resistance when a large pressure is applied, making it difficult for them to be pressed into the magnetic layer, and S 1.6 tends to be large. And S 0.1 and S 1.6 By controlling the difference (S 0.1 -S 1.6) can be reduced to 32 nm or less.

[0058] The abrasive, which is another form of the nonmagnetic filler, is preferably a nonmagnetic powder having a Mohs hardness of more than 8, and more preferably a nonmagnetic powder having a Mohs hardness of 9 or more. In contrast, the Mohs hardness of the protrusion-forming agent can be, for example, 8 or less or 7 or less. The maximum value of the Mohs hardness is 10, which is the same as that of diamond. Specifically, the abrasive can be alumina (Al2O3), silicon carbide, boron carbide (B4C), SiO2, TiC, chromium oxide (Cr2O3), cerium oxide, zirconium oxide (ZrO2), iron oxide, diamond, and other powders, and among these, alumina powder such as α-alumina and silicon carbide powder are preferred. The average particle size of the abrasive can be, for example, in the range of 30 to 300 nm, and is preferably in the range of 50 to 200 nm.

[0059] From the viewpoint of allowing the protrusion-forming agent and the abrasive to better exert their functions, the content of the protrusion-forming agent in the magnetic layer is preferably 0.1 to 5.0 parts by mass, and more preferably 0.3 to 3.5 parts by mass, relative to 100.0 parts by mass of the ferromagnetic powder. On the other hand, the content of the abrasive in the magnetic layer is preferably 1.0 to 20.0 parts by mass, and more preferably 3.0 to 15.0 parts by mass, and even more preferably 4.0 to 10.0 parts by mass, relative to 100.0 parts by mass of the ferromagnetic powder.

[0060] As an example of an additive that can be used in the magnetic layer containing an abrasive, the dispersant described in paragraphs 0012 to 0022 of JP 2013-131285 A can be mentioned as a dispersant for improving the dispersibility of the abrasive in the magnetic layer forming composition. For the dispersant, refer to paragraphs 0061 and 0071 of JP 2012-133837 A. The dispersant may be contained in the non-magnetic layer. For the dispersant that can be contained in the non-magnetic layer, refer to paragraph 0061 of JP 2012-133837 A.

[0061] The lubricant, which is one embodiment of an additive that can be contained in the magnetic layer, can be one or more lubricants selected from the group consisting of fatty acids, fatty acid esters, and fatty acid amides. 0.1 and S 1.6 is a value obtained by measuring the spacing on the magnetic layer surface after cleaning with n-hexane. If a liquid film of lubricant is present on the surface of the magnetic layer that is pressed during spacing measurement, the measured spacing will be narrower by the thickness of this liquid film. In contrast, it is presumed that the lubricant that may be present as a liquid film during pressing can be removed by cleaning with n-hexane. Therefore, it is considered that by measuring the spacing after cleaning with n-hexane, a spacing value can be obtained that corresponds well to the state of the protrusions (protrusion height) on the magnetic layer surface.

[0062] Examples of fatty acids include lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, behenic acid, erucic acid, elaidic acid, etc., with stearic acid, myristic acid, and palmitic acid being preferred, and stearic acid being more preferred. The fatty acid may be contained in the magnetic layer in the form of a salt such as a metal salt. Examples of fatty acid esters include esters of lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, behenic acid, erucic acid, elaidic acid, etc. Specific examples include butyl myristate, butyl palmitate, butyl stearate (butyl stearate), neopentyl glycol dioleate, sorbitan monostearate, sorbitan distearate, sorbitan tristearate, oleyl oleate, isocetyl stearate, isotridecyl stearate, octyl stearate, isooctyl stearate, amyl stearate, butoxyethyl stearate, etc. Examples of the fatty acid amide include amides of the above-mentioned various fatty acids, such as lauric acid amide, myristic acid amide, palmitic acid amide, and stearic acid amide. As for fatty acids and fatty acid derivatives (amides, esters, etc.), it is preferable that the fatty acid-derived portion of the fatty acid derivative has a structure similar to or similar to that of the fatty acid used in combination. For example, when stearic acid is used as the fatty acid, it is preferable to use a stearic acid ester and / or a stearic acid amide. The fatty acid content of the magnetic layer is, for example, 0 to 10.0 parts by mass, preferably 0.1 to 10.0 parts by mass, and more preferably 1.0 to 7.0 parts by mass per 100.0 parts by mass of the ferromagnetic powder. The fatty acid ester content of the magnetic layer is, for example, 0 to 10.0 parts by mass, preferably 0.1 to 10.0 parts by mass, and more preferably 1.0 to 7.0 parts by mass per 100.0 parts by mass of the ferromagnetic powder. The fatty acid amide content of the magnetic layer is, for example, 0 to 3.0 parts by mass, preferably 0 to 2.0 parts by mass, and more preferably 0 to 1.0 parts by mass per 100.0 parts by mass of the ferromagnetic powder. In addition, when the magnetic tape has a non-magnetic layer between the non-magnetic support and the magnetic layer, the fatty acid content of the non-magnetic layer is, for example, 0 to 10.0 parts by mass, preferably 1.0 to 10.0 parts by mass, and more preferably 1.0 to 7.0 parts by mass per 100.0 parts by mass of non-magnetic powder. The fatty acid ester content of the non-magnetic layer is, for example, 0 to 15.0 parts by mass, and preferably 0.1 to 10.0 parts by mass, per 100.0 parts by mass of non-magnetic powder. The fatty acid amide content of the non-magnetic layer is, for example, 0 to 3.0 parts by mass, and preferably 0 to 1.0 parts by mass, per 100.0 parts by mass of non-magnetic powder.

[0063] <Nonmagnetic layer> Next, the non-magnetic layer will be described. The magnetic tape may have a magnetic layer directly on the non-magnetic support, or may have a non-magnetic layer containing a non-magnetic powder between the non-magnetic support and the magnetic layer. The non-magnetic powder used in the non-magnetic layer may be a powder of an inorganic substance (inorganic powder) or a powder of an organic substance (organic powder). Carbon black and the like can also be used. Examples of inorganic substances include metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, and metal sulfides. These non-magnetic powders are commercially available, and can also be produced by known methods. For details, refer to paragraphs 0146 to 0150 of JP-A-2011-216149. For carbon black that can be used in the non-magnetic layer, refer to paragraphs 0040 to 0041 of JP-A-2010-24113. The content (filling rate) of the non-magnetic powder in the non-magnetic layer is preferably in the range of 50 to 90% by mass, and more preferably in the range of 60 to 90% by mass.

[0064] The non-magnetic layer may contain a binder and may also contain an additive. For other details of the binder, additive, etc. of the non-magnetic layer, known techniques related to non-magnetic layers can be applied. In addition, for example, for the type and content of the binder, the type and content of the additive, known techniques related to magnetic layers can also be applied.

[0065] The non-magnetic layer of the magnetic tape includes a substantially non-magnetic layer that contains a small amount of ferromagnetic powder, for example as an impurity or intentionally, along with the non-magnetic powder. A substantially non-magnetic layer here refers to a layer having a residual magnetic flux density of 10 mT or less, a coercive force of 7.96 kA / m (100 Oe) or less, or a layer having a residual magnetic flux density of 10 mT or less and a coercive force of 7.96 kA / m (100 Oe) or less. It is preferable that the non-magnetic layer has no residual magnetic flux density or coercive force.

[0066] <Nonmagnetic support> Next, the non-magnetic support will be described. Examples of the non-magnetic support (hereinafter, simply referred to as "support") include known biaxially stretched polyethylene terephthalate, polyethylene naphthalate, polyamide, polyamideimide, aromatic polyamide, and the like. Among these, polyethylene terephthalate, polyethylene naphthalate, and polyamide are preferred. These supports may be previously subjected to corona discharge, plasma treatment, easy-adhesion treatment, heat treatment, and the like.

[0067] <Backcoat layer> The tape may or may not have a backcoat layer containing a nonmagnetic powder on the surface side opposite to the surface side having the magnetic layer of the nonmagnetic support. The backcoat layer preferably contains one or both of carbon black and inorganic powder. The backcoat layer may contain a binder and may also contain additives. For details of the binder, additives, etc. of the backcoat layer, known techniques related to the backcoat layer may be applied, and known techniques related to the magnetic layer and / or nonmagnetic layer may also be applied. For example, the descriptions of paragraphs 0018 to 0020 of JP 2006-331625 A and US Pat. No. 7,029,774, column 4, line 65 to column 5, line 38, may be referred to for the backcoat layer.

[0068] <Various thicknesses> Regarding the thickness (total thickness) of the magnetic tape, with the enormous increase in the amount of information in recent years, there is a demand for magnetic tapes to have higher recording capacity (higher capacity). One way to increase capacity is to reduce the thickness of the magnetic tape and increase the length of the magnetic tape contained in one magnetic tape cartridge. From this point of view, the thickness (total thickness) of the magnetic tape is preferably 5.6 μm or less, more preferably 5.5 μm or less, more preferably 5.4 μm or less, and even more preferably 5.3 μm or less. From the viewpoint of ease of handling, the thickness of the magnetic tape is preferably 3.0 μm or more, and more preferably 3.5 μm or more.

[0069] The thickness (total thickness) of the magnetic tape can be measured by the following method. Ten tape samples (e.g., 5 to 10 cm long) are cut out from any part of the magnetic tape, and the tape samples are stacked and the thickness is measured. The measured thickness is divided by 10 to obtain the value (thickness per tape sample), which is the tape thickness. The thickness measurement can be performed using a known measuring device capable of measuring thickness to the order of 0.1 μm.

[0070] The thickness of the non-magnetic support is preferably 3.0 to 5.0 μm. The thickness of the magnetic layer can be optimized according to the saturation magnetization amount of the magnetic head used, the head gap length, the band of the recording signal, etc., and is generally 0.01 μm to 0.15 μm, and from the viewpoint of high-density recording, is preferably 0.02 μm to 0.12 μm, and more preferably 0.03 μm to 0.1 μm. At least one magnetic layer is sufficient, and the magnetic layer may be separated into two or more layers having different magnetic properties, and a known configuration related to a multilayer magnetic layer can be applied. When the magnetic layer is separated into two or more layers, the thickness of the magnetic layer is the total thickness of these layers. The thickness of the nonmagnetic layer is, for example, 0.1 to 1.5 μm, and preferably 0.1 to 1.0 μm. The thickness of the backcoat layer is preferably 0.9 μm or less, and more preferably 0.1 to 0.7 μm. Various thicknesses such as the thickness of the magnetic layer can be determined by the following method. A cross section of the magnetic tape in the thickness direction is exposed by an ion beam, and then the exposed cross section is observed by a scanning electron microscope. Various thicknesses can be obtained as the arithmetic average of thicknesses obtained at any two points in the cross section observation. Alternatively, various thicknesses can be obtained as design thicknesses calculated from manufacturing conditions, etc.

[0071] <Manufacturing method> (Preparation of compositions for forming each layer) The composition for forming the magnetic layer, non-magnetic layer or backcoat layer usually contains a solvent in addition to the various components described above. As the solvent, various organic solvents generally used for manufacturing coating-type magnetic recording media can be used. Among them, from the viewpoint of the solubility of the binder generally used in coating-type magnetic recording media, it is preferable that each layer-forming composition contains one or more ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, diisobutyl ketone, cyclohexanone, isophorone, and tetrahydrofuran. The amount of solvent in each layer-forming composition is not particularly limited, and can be the same as that of each layer-forming composition of a normal coating-type magnetic recording medium. In addition, the process for preparing each layer-forming composition can usually include at least a kneading process, a dispersing process, and a mixing process provided before or after these processes as necessary. Each individual process may be divided into two or more stages. The components used in the preparation of each layer-forming composition may be added at the beginning or during any process. In addition, each component may be added in two or more steps in a divided manner. For example, the binder may be added in portions in the kneading step, the dispersing step, and the mixing step for adjusting the viscosity after dispersion. In the manufacturing process of the magnetic tape, conventional known manufacturing techniques may be used in some or all of the steps. In the kneading step, it is preferable to use a kneader having a strong kneading force, such as an open kneader, a continuous kneader, a pressure kneader, or an extruder. Details of these kneading processes are described in JP-A-1-106338 and JP-A-1-79274. In addition, glass beads and / or other beads may be used to disperse the composition for forming each layer. As such dispersing beads, zirconia beads, titania beads, and steel beads, which are dispersing beads with high specific gravity, are suitable. It is preferable to use these dispersing beads with an optimized particle size (bead diameter) and packing rate. A known dispersing machine may be used. Each layer forming composition may be filtered by a known method before being subjected to the coating step. Filtration can be performed, for example, by filter filtration.The filter used for filtration may be, for example, a filter with a pore size of 0.01 to 3 μm (eg, a glass fiber filter, a polypropylene filter, etc.).

[0072] (Coating process) The magnetic layer can be formed, for example, by directly applying the magnetic layer forming composition onto a non-magnetic support, or by sequentially or simultaneously applying a multi-layer coating with the non-magnetic layer forming composition. In an embodiment in which an orientation treatment is performed, the coating layer of the magnetic layer forming composition is oriented in the orientation zone while the coating layer is in a wet state. For the orientation treatment, various known techniques, including those described in paragraph 0052 of JP-A-2010-24113, can be applied. For example, the vertical orientation treatment can be performed by a known method, such as a method using magnets with different poles facing each other. In the orientation zone, the drying speed of the coating layer can be controlled by the temperature and volume of the drying air and / or the conveying speed in the orientation zone. The coating layer may also be pre-dried before being conveyed to the orientation zone. The backcoat layer can be formed by applying a composition for forming a backcoat layer to the side of the non-magnetic support opposite to the side having the magnetic layer (or the side on which the magnetic layer will be formed later). For details of the coating for forming each layer, see paragraph 0066 of JP2010-231843A.

[0073] (Other processes) After the above coating step, a calendering process is usually carried out to improve the surface smoothness of the magnetic tape. The stronger the calendering conditions, the lower the height of the protrusions formed by the protrusion-forming agent on the magnetic layer surface of the manufactured magnetic tape. This results in, for example, S 0.1can be reduced. Calendaring conditions include the type and number of stages of calendar rolls, calendar pressure, calendar temperature (surface temperature of calendar rolls), calendar speed, etc. Calendaring pressure is, for example, 200 to 500 kN / m, preferably 250 to 350 kN / m, calendar temperature is, for example, 70 to 120°C, preferably 80 to 100°C, and calendar speed is, for example, 50 to 300 m / min, preferably 80 to 200 m / min. In addition, the harder the surface of the calendar rolls used and the more stages are increased, the smoother the magnetic layer surface tends to be, so the height of the protrusions on the magnetic layer surface can also be adjusted by the combination of calendar rolls and the number of stages. For other various steps in manufacturing the magnetic tape, reference can be made to paragraphs 0067 to 0070 of JP2010-231843A. A long magnetic tape roll can be obtained through various processes. The obtained magnetic tape roll is cut (slit) to the width of the magnetic tape to be housed in a magnetic tape cartridge by a known cutter. The width can be determined according to standards and is usually 1 / 2 inch. 1 / 2 inch = 12.65 mm. A servo pattern is usually formed on the magnetic tape obtained by slitting.

[0074] (Formation of servo pattern) “Formation of a servo pattern” can also be called “recording of a servo signal.” The formation of a servo pattern will be described below.

[0075] The servo pattern is usually formed along the longitudinal direction of the magnetic tape. Methods of control using servo signals (servo control) include timing-based servo (TBS), amplitude servo, and frequency servo.

[0076] As shown in ECMA (European Computer Manufacturers Association)-319 (June 2001), magnetic tapes (generally called "LTO tapes") conforming to the LTO (Linear Tape-Open) standard employ a timing-based servo system. In this timing-based servo system, a servo pattern is formed by a pair of non-parallel magnetic stripes (also called "servo stripes") arranged continuously in the longitudinal direction of the magnetic tape. In this invention and this specification, the "timing-based servo pattern" refers to a servo pattern that enables head tracking in a servo system of the timing-based servo system. As described above, the servo pattern is formed by a pair of non-parallel magnetic stripes in order to inform the servo signal reading element passing over the servo pattern of its passing position. Specifically, the pair of magnetic stripes is formed so that the interval between them changes continuously along the width direction of the magnetic tape, and the servo signal reading element can know the relative position between the servo pattern and the servo signal reading element by reading the interval. This relative position information enables tracking of the data track. For this reason, a plurality of servo tracks are usually set on the servo pattern along the width direction of the magnetic tape.

[0077] A servo band is made up of a continuous servo pattern in the longitudinal direction of the magnetic tape. Usually, multiple servo bands are provided on a magnetic tape. For example, there are five servo bands on an LTO tape. The area between two adjacent servo bands is the data band. The data band is made up of multiple data tracks, and each data track corresponds to one servo track.

[0078] Also, in one embodiment, as shown in JP 2004-318983 A, information indicating the number of the servo band (also called "servo band ID (identification)" or "UDIM (Unique Data Band Identification Method) information") is embedded in each servo band. This servo band ID is recorded by shifting a specific one of a plurality of pairs of servo stripes in the servo band so that its position is displaced relatively in the longitudinal direction of the magnetic tape. Specifically, the way in which a specific one of a plurality of pairs of servo stripes is shifted is changed for each servo band. As a result, the recorded servo band ID is unique for each servo band, so that the servo band can be uniquely identified simply by reading one servo band with a servo signal reading element.

[0079] As a method for uniquely identifying servo bands, there is also a method using the staggered method as shown in ECMA-319 (June 2001). In this staggered method, a group of pairs of non-parallel magnetic stripes (servo stripes) arranged continuously in the longitudinal direction of the magnetic tape are recorded so that they are shifted in the longitudinal direction of the magnetic tape for each servo band. The combination of the shift between adjacent servo bands is unique across the entire magnetic tape, so when the servo pattern is read by two servo signal reading elements, it is possible to uniquely identify the servo bands.

[0080] Also, as specified in ECMA-319 (June 2001), information indicating the longitudinal position of the magnetic tape (also called "LPOS (Longitudinal Position) information") is usually embedded in each servo band. Like UDIM information, this LPOS information is also recorded by shifting the positions of a pair of servo stripes in the longitudinal direction of the magnetic tape. However, unlike UDIM information, the same signal is recorded in each servo band with this LPOS information.

[0081] It is also possible to embed information other than the above UDIM information and LPOS information in the servo bands. In this case, the embedded information may be different for each servo band, such as UDIM information, or may be common to all servo bands, such as LPOS information. Also, methods other than those described above can be used to embed information in the servo bands. For example, a predetermined code may be recorded by thinning out a predetermined pair from a group of pairs of servo stripes.

[0082] The head for forming a servo pattern is called a servo write head. The servo write head usually has a pair of gaps corresponding to the pair of magnetic stripes, the number of which is equal to the number of servo bands. Usually, a core and a coil are connected to each pair of gaps, and a magnetic field generated in the core can generate a leakage magnetic field in the pair of gaps by supplying a current pulse to the coil. When forming a servo pattern, a magnetic pattern corresponding to the pair of gaps can be transferred to the magnetic tape by inputting a current pulse while running the magnetic tape on the servo write head, thereby forming the servo pattern. The width of each gap can be appropriately set according to the density of the servo pattern to be formed. The width of each gap can be set, for example, to 1 μm or less, 1 to 10 μm, or 10 μm or more.

[0083] Before forming a servo pattern on the magnetic tape, the magnetic tape is usually subjected to a demagnetization (erase) process. This erase process can be performed by applying a uniform magnetic field to the magnetic tape using a direct current magnet or an alternating current magnet. There are two types of erase processes: DC (Direct Current) erase and AC (Alternating Current) erase. AC erase is performed by gradually lowering the strength of the magnetic field applied to the magnetic tape while reversing the direction of the magnetic field. On the other hand, DC erase is performed by applying a unidirectional magnetic field to the magnetic tape. There are two more methods of DC erase. The first method is horizontal DC erase, which applies a unidirectional magnetic field along the longitudinal direction of the magnetic tape. The second method is vertical DC erase, which applies a unidirectional magnetic field along the thickness direction of the magnetic tape. The erase process may be performed on the entire magnetic tape, or may be performed for each servo band of the magnetic tape.

[0084] The direction of the magnetic field of the formed servo pattern is determined according to the direction of erasure. For example, when the magnetic tape is subjected to horizontal DC erasure, the servo pattern is formed so that the direction of the magnetic field is opposite to the direction of erasure. This makes it possible to increase the output of the servo signal obtained by reading the servo pattern. As shown in JP2012-53940A, when the magnetic pattern is transferred to the magnetic tape that has been vertically DC erased using the above gap, the servo signal obtained by reading the formed servo pattern has a unipolar pulse shape. On the other hand, when the magnetic pattern is transferred to the magnetic tape that has been horizontally DC erased using the above gap, the servo signal obtained by reading the formed servo pattern has a bipolar pulse shape.

[0085] [Magnetic tape cartridge] One aspect of the present invention relates to a magnetic tape cartridge including the above-mentioned magnetic tape.

[0086] The details of the magnetic tape contained in the magnetic tape cartridge are as described above.

[0087] In a magnetic tape cartridge, the magnetic tape is generally accommodated inside the cartridge body in a state where it is wound around a reel. The reel is provided rotatably inside the cartridge body. As the magnetic tape cartridge, a single-reel type magnetic tape cartridge having one reel inside the cartridge body and a twin-reel type magnetic tape cartridge having two reels inside the cartridge body are widely used. When a single-reel type magnetic tape cartridge is loaded into a magnetic tape device for recording and / or reproducing data on the magnetic tape, the magnetic tape is pulled out from the magnetic tape cartridge and wound around the reel on the magnetic tape device side. A magnetic head is disposed on the magnetic tape transport path from the magnetic tape cartridge to the take-up reel. The magnetic tape is fed and wound between the reel (supply reel) on the magnetic tape cartridge side and the reel (take-up reel) on the magnetic tape device side. During this time, the magnetic head comes into contact with and slides on the surface of the magnetic layer of the magnetic tape, thereby recording and / or reproducing data. In contrast, a dual-reel magnetic tape cartridge is provided with both a supply reel and a take-up reel inside the magnetic tape cartridge.

[0088] In one embodiment, the magnetic tape cartridge may include a cartridge memory. The cartridge memory may be, for example, a non-volatile memory, and may be a memory in which tension adjustment information is already recorded, or a memory in which tension adjustment information is to be recorded. The tension adjustment information is information for adjusting the tension applied in the longitudinal direction of the magnetic tape. For more information on the cartridge memory, please refer to the description below.

[0089] The above magnetic tape and magnetic tape cartridge can be suitably used in a magnetic tape device (in other words, a magnetic recording and reproducing system) that controls the width of the magnetic tape by adjusting the tension applied to the magnetic tape in the longitudinal direction.

[0090] [Magnetic tape device] One aspect of the present invention relates to a magnetic tape device including a magnetic tape cartridge. In the magnetic tape device, data can be recorded on the magnetic tape and / or data recorded on the magnetic tape can be reproduced by bringing a magnetic head into contact with the surface of the magnetic layer of the magnetic tape and sliding the magnetic head. The magnetic tape device can detachably include the magnetic tape cartridge according to one aspect of the present invention.

[0091] The magnetic tape cartridge can be mounted in a magnetic tape device equipped with a magnetic head and used to record and / or reproduce data. In the present invention and this specification, the term "magnetic tape device" refers to a device capable of recording data on a magnetic tape and / or reproducing data recorded on the magnetic tape. Such a device is generally called a drive. The magnetic head included in the magnetic tape device can be a recording head capable of recording data on the magnetic tape, and can also be a reproducing head capable of reproducing data recorded on the magnetic tape. In one embodiment, the magnetic tape device can include both a recording head and a reproducing head as separate magnetic heads. In another embodiment, the magnetic head included in the magnetic tape device can have a configuration in which both a recording element and a reproducing element are provided in one magnetic head. As the reproducing head, a magnetic head (MR head) that includes a magnetoresistive (MR) element as a reproducing element capable of reading information recorded on a magnetic tape with good sensitivity is preferable. As the MR head, various known MR heads (for example, a GMR (Giant Magnetoresistive) head, a TMR (Tunnel Magnetoresistive) head, etc.) can be used. A servo pattern reading element may be included in the magnetic head that records and / or reproduces data. Alternatively, a magnetic head (servo head) equipped with a servo pattern reading element may be included in the magnetic tape device as a head separate from the magnetic head that records and / or reproduces data. For example, a magnetic head that records and / or reproduces recorded data (hereinafter also referred to as a "recording and reproducing head") may include two servo signal reading elements, and each of the two servo signal reading elements can simultaneously read two adjacent servo bands sandwiching a data band. One or more data elements may be disposed between the two servo signal reading elements. An element for recording data (a recording element) and an element for reproducing data (a reproducing element) are collectively referred to as a "data element".

[0092] By using a reproducing element with a narrow reproducing element width as the reproducing element to reproduce data, data recorded at a high density can be reproduced with high sensitivity. From this viewpoint, the reproducing element width of the reproducing element is preferably 0.8 μm or less. The reproducing element width of the reproducing element can be, for example, 0.3 μm or more. However, from the above viewpoint, it is also preferable that the reproducing element width is less than this value. On the other hand, the narrower the reproducing element width, the more likely it is that phenomena such as reproduction failure due to off-track will occur. In order to suppress the occurrence of such phenomena, a magnetic tape device that controls the dimension of the magnetic tape in the width direction by adjusting the tension applied in the longitudinal direction of the magnetic tape is preferable. Here, the "reading element width" refers to the physical dimension of the reading element width. Such physical dimension can be measured using an optical microscope, a scanning electron microscope, or the like.

[0093] When recording data and / or reproducing recorded data, tracking can be performed using servo signals first. That is, by making the servo signal reading element follow a specific servo track, the data element can be controlled to pass over the target data track. The data track is moved by changing the servo track read by the servo signal reading element in the tape width direction. The recording / reproducing head can also record and / or reproduce data on other data bands by using the UDIM information described above to move the servo signal reading element to a specific servo band and start tracking on that servo band.

[0094] FIG. 1 shows an example of the arrangement of data bands and servo bands. In FIG. 1, a plurality of servo bands 1 are arranged on the magnetic layer of the magnetic tape MT, sandwiched between guide bands 3. A plurality of regions 2 sandwiched between two servo bands are data bands. A servo pattern is a magnetized region, and is formed by magnetizing a specific region of the magnetic layer with a servo write head. The region magnetized by the servo write head (the position where the servo pattern is formed) is determined by a standard. For example, in an LTO Ultrium format tape, which is an industry standard, a plurality of servo patterns inclined with respect to the tape width direction are formed on the servo band during the manufacturing of the magnetic tape, as shown in FIG. 2. More specifically, in FIG. 2, a servo frame SF on the servo band 1 is composed of a servo subframe 1 (SSF1) and a servo subframe 2 (SSF2). The servo subframe 1 is composed of an A burst (symbol A in FIG. 2) and a B burst (symbol B in FIG. 2). The A burst is composed of servo patterns A1 to A5, and the B burst is composed of servo patterns B1 to B5. On the other hand, the servo subframe 2 is composed of a C burst (symbol C in FIG. 2) and a D burst (symbol D in FIG. 2). The C burst is composed of servo patterns C1 to C4, and the D burst is composed of servo patterns D1 to D4. Such 18 servo patterns are arranged in a subframe arranged in a 5, 5, 4, 4 arrangement in a set of 5 and 4, and are used to identify a servo frame. For the sake of explanation, one servo frame is shown in FIG. 2. However, in reality, a plurality of servo frames are arranged in the running direction in each servo band on the magnetic layer of a magnetic tape where head tracking of the timing-based servo method is performed. In FIG. 2, the arrow indicates the running direction. For example, an LTO Ultrium format tape usually has 5,000 or more servo frames per meter of tape length in each servo band on the magnetic layer.

[0095] The magnetic tape device preferably has a tension adjustment mechanism for controlling the width dimension of the magnetic tape by adjusting the tension applied to the magnetic tape in the longitudinal direction. An example of such a magnetic tape device will be described below with reference to Fig. 3. However, the present invention is not limited to the example shown in Fig. 3.

[0096] <Magnetic tape device configuration> A magnetic tape device 10 shown in FIG. 3 controls a recording / reproducing head unit 12 in response to commands from a control device 11, and records and reproduces data on a magnetic tape MT. The magnetic tape device 10 has a configuration capable of detecting and adjusting tension applied to the magnetic tape in the longitudinal direction from spindle motors 17A, 17B that control the rotation of the magnetic tape cartridge reel and take-up reel and their drive devices 18A, 18B. The magnetic tape device 10 has a configuration in which a magnetic tape cartridge 13 can be loaded. The magnetic tape device 10 has a cartridge memory read / write device 14 capable of reading from and writing to a cartridge memory 131 in the magnetic tape cartridge 13 . From the magnetic tape cartridge 13 attached to the magnetic tape device 10, the end or leader pin of the magnetic tape MT is pulled out by an automatic loading mechanism or manually, and the magnetic tape MT passes over the recording / playback head via guide rollers 15A and 15B with the magnetic layer surface in a direction facing the recording / playback head surface of the recording / playback head unit 12, and the magnetic tape MT is taken up onto the take-up reel 16. The rotation and torque of spindle motors 17A and 17B are controlled by signals from control device 11, and magnetic tape MT runs at any speed and tension. A servo pattern formed in advance on the magnetic tape can be used to control the tape speed. A tension detection mechanism may be provided between magnetic tape cartridge 13 and take-up reel 16 to detect tension. Tension control may be performed using guide rollers 15A and 15B in addition to control by spindle motors 17A and 17B. The cartridge memory read / write device 14 is configured to be able to read and write information from and to the cartridge memory 131 in response to commands from the control device 11. As a communication method between the cartridge memory read / write device 14 and the cartridge memory 131, for example, the ISO (International Organization for Standardization) 14443 method can be adopted.

[0097] The control device 11 includes, for example, a control unit, a storage unit, a communication unit, and the like.

[0098] The recording and reproducing head unit 12 is composed of, for example, a recording and reproducing head, a servo tracking actuator that adjusts the position of the recording and reproducing head in the track width direction, a recording and reproducing amplifier 19, a connector cable for connecting to the control device 11, etc. The recording and reproducing head is composed of, for example, a recording element that records data on the magnetic tape, a reproducing element that reproduces the data on the magnetic tape, and a servo signal reading element that reads the servo signal recorded on the magnetic tape. One magnetic head is equipped with, for example, one or more of each of the recording element, reproducing element, and servo signal reading element. Alternatively, each element may be provided separately in a plurality of magnetic heads according to the running direction of the magnetic tape.

[0099] The recording / reproducing head unit 12 is configured to be capable of recording data onto the magnetic tape MT in response to a command from the control device 11. Also, the recording / reproducing head unit 12 is configured to be capable of reproducing the data recorded onto the magnetic tape MT in response to a command from the control device 11.

[0100] The control device 11 has a mechanism for determining the running position of the magnetic tape MT from the servo signal read from the servo band while the magnetic tape MT is running, and for controlling the servo tracking actuator so that the recording element and / or the reproducing element are positioned at the target running position (track position). This control of the track position is performed, for example, by feedback control. The control device 11 has a mechanism for determining the servo band interval from the servo signals read from two adjacent servo bands while the magnetic tape MT is running. The control device 11 also has a mechanism for controlling the torque of the spindle motor 17A and the spindle motor 17B and / or the guide rollers 15A and 15B to control the tension in the longitudinal direction of the magnetic tape so that the servo band interval becomes a target value. This tension control is performed, for example, by feedback control. The control device 11 can also store information on the determined servo band interval in a storage unit inside the control device 11, a cartridge memory 131, an external connected device, or the like. EXAMPLES

[0101] The present invention will be described below based on examples. However, the present invention is not limited to the embodiments shown in the examples. "Parts" described below refer to "parts by mass". Furthermore, the steps and evaluations described below were carried out in an environment with an atmospheric temperature of 23°C ± 1°C unless otherwise specified. "eq" described below is equivalent, and is a unit that cannot be converted to SI units.

[0102] The protrusion-forming agents used in the manufacture of the magnetic tapes of the Examples and Comparative Examples are as follows. Protrusion-Forming Agent 1 and Protrusion-Forming Agent 3 are particles with low surface smoothness. Protrusion-Forming Agent 2 has a cocoon-like particle shape. Protrusion-Forming Agent 4 has a nearly spherical particle shape. Protrusion forming agent 1: ATLAS (composite particles of silica and polymer) manufactured by Cabot Corporation, average particle size 100 nm Protrusion forming agent 2: Cabot TGC6020N (silica particles), average particle size 140 nm Protrusion-forming agent 3: Cataloid (water-dispersed sol of silica particles; the water-dispersed sol was heated to remove the solvent and the resulting dried product was used as the protrusion-forming agent for preparing the protrusion-forming agent liquid described below), manufactured by JGC Catalysts and Chemicals, average particle size 120 nm Protrusion-forming agent 4: PL-10L manufactured by Fuso Chemical Co., Ltd. (water-dispersed sol of silica particles; the water-dispersed sol was heated to remove the solvent and the resulting dried product was used as the protrusion-forming agent for preparing the protrusion-forming agent liquid described below), average particle size 130 nm

[0103] In Table 1, "BaFe" is hexagonal barium ferrite powder (coercive force Hc: 196 kA / m, average particle size (average plate diameter): 24 nm).

[0104] In Table 1, "SrFe1" is a hexagonal strontium ferrite powder produced by the following method. 1707 g of SrCO3, 687 g of H3BO3, 1120 g of Fe2O3, 45 g of Al(OH)3, 24 g of BaCO3, 13 g of CaCO3, and 235 g of Nd2O3 were weighed out and mixed in a mixer to obtain a raw material mixture. The obtained raw material mixture was melted in a platinum crucible at a melting temperature of 1390°C, and the melt was poured into a rod shape at about 6 g / sec by heating the tapping hole at the bottom of the platinum crucible while stirring the melt. The tapped liquid was rolled and quenched with a water-cooled twin roller to produce an amorphous body. 280 g of the produced amorphous body was placed in an electric furnace, heated to 635°C (crystallization temperature) at a heating rate of 3.5°C / min, and held at that temperature for 5 hours to precipitate (crystallize) hexagonal strontium ferrite particles. Next, the crystallized material obtained above containing hexagonal strontium ferrite particles was coarsely crushed in a mortar, and 1000 g of zirconia beads with a particle size of 1 mm and 800 ml of 1% aqueous acetic acid solution were added to a glass bottle and dispersed for 3 hours using a paint shaker. The resulting dispersion was then separated from the beads and placed in a stainless steel beaker. The dispersion was left to stand at a liquid temperature of 100°C for 3 hours to dissolve the glass components, and then precipitated in a centrifuge and washed by repeated decantation, and dried for 6 hours in a heating furnace at a furnace temperature of 110°C to obtain hexagonal strontium ferrite powder. The average particle size of the hexagonal strontium ferrite powder obtained above is 18 nm, and the activation volume is 902 nm. 3 , the anisotropy constant Ku is 2.2×10 5 J / m3 , mass magnetization σs is 49A m 2 / kg. A 12 mg sample powder was taken from the hexagonal strontium ferrite powder obtained above, and this sample powder was partially dissolved under the dissolution conditions exemplified above. The elemental analysis of the filtrate obtained was performed using an ICP analyzer to determine the surface layer content of neodymium atoms. Separately, 12 mg of sample powder was taken from the hexagonal strontium ferrite powder obtained above, and this sample powder was completely dissolved under the dissolution conditions exemplified above. The elemental analysis of the filtrate obtained was performed using an ICP analyzer to determine the bulk content of neodymium atoms. The neodymium atom content (bulk content) relative to 100 atomic % of iron atoms in the hexagonal strontium ferrite powder obtained above was 2.9 atomic %. The surface layer content of neodymium atoms was 8.0 atomic %. The ratio of the surface layer content to the bulk content, "surface layer content / bulk content," was 2.8, confirming that neodymium atoms were unevenly distributed in the surface layers of the particles. It was confirmed that the powder obtained above exhibited a hexagonal ferrite crystal structure by scanning with CuKα radiation at a voltage of 45 kV and an intensity of 40 mA and measuring the X-ray diffraction pattern under the following conditions (X-ray diffraction analysis). The powder obtained above exhibited a magnetoplumbite-type (M-type) hexagonal ferrite crystal structure. The crystal phase detected by the X-ray diffraction analysis was a single phase of magnetoplumbite type. PANalytical X'Pert Pro diffractometer, PIXcel detector Soller slits for incident and diffracted beams: 0.017 radians Dispersion slit fixed angle: 1 / 4 degree Mask: 10mm Anti-scatter slit: 1 / 4 degree Measurement mode: Continuous Measurement time per step: 3 seconds Measurement speed: 0.017 degrees per second Measurement step: 0.05 degrees

[0105] In Table 1, "SrFe2" is a hexagonal strontium ferrite powder produced by the following method. 1725 g of SrCO3, 666 g of H3BO3, 1332 g of Fe2O3, 52 g of Al(OH)3, 34 g of CaCO3, and 141 g of BaCO3 were weighed out and mixed in a mixer to obtain a raw material mixture. The obtained raw material mixture was melted in a platinum crucible at a melting temperature of 1380°C, and the melt was poured into a rod shape at about 6 g / sec by heating the tapping hole at the bottom of the platinum crucible while stirring the melt. The tapped liquid was quenched and rolled with a water-cooled twin roll to produce an amorphous body. 280 g of the obtained amorphous body was placed in an electric furnace, heated to 645° C. (crystallization temperature), and held at that temperature for 5 hours to precipitate (crystallize) hexagonal strontium ferrite particles. Next, the crystallized material obtained above containing hexagonal strontium ferrite particles was coarsely crushed in a mortar, and 1000 g of zirconia beads with a particle size of 1 mm and 800 ml of 1% aqueous acetic acid solution were added to a glass bottle and dispersed for 3 hours using a paint shaker. The resulting dispersion was then separated from the beads and placed in a stainless steel beaker. The dispersion was left to stand at a liquid temperature of 100°C for 3 hours to dissolve the glass components, and then precipitated in a centrifuge and washed by repeated decantation, and dried for 6 hours in a heating furnace at a furnace temperature of 110°C to obtain hexagonal strontium ferrite powder. The average particle size of the obtained hexagonal strontium ferrite powder was 19 nm, and the activation volume was 1102 nm. 3 , the anisotropy constant Ku is 2.0×10 5 J / m 3 , mass magnetization σs is 50A m 2 / kg.

[0106] In Table 1, "ε-iron oxide" is ε-iron oxide powder prepared by the following method. 8.3g of iron (III) nitrate nonahydrate, 1.3g of gallium (III) nitrate octahydrate, 190mg of cobalt (II) nitrate hexahydrate, 150mg of titanium (IV) sulfate, and 1.5g of polyvinylpyrrolidone (PVP) were dissolved in 90g of pure water, and 4.0g of ammonia solution with a concentration of 25% was added under the condition of an atmospheric temperature of 25°C while stirring with a magnetic stirrer in the air atmosphere, and the mixture was stirred for 2 hours at an atmospheric temperature of 25°C. A citric acid solution obtained by dissolving 1g of citric acid in 9g of pure water was added to the obtained solution, and the mixture was stirred for 1 hour. The powder precipitated after stirring was collected by centrifugation, washed with pure water, and dried in a heating furnace at an internal temperature of 80°C. 800g of pure water was added to the dried powder, and the powder was dispersed in water again to obtain a dispersion. The obtained dispersion was heated to 50°C, and 40g of 25% ammonia aqueous solution was added dropwise while stirring. After stirring for 1 hour while maintaining the temperature at 50°C, 14mL of tetraethoxysilane (TEOS) was added dropwise and stirred for 24 hours. 50g of ammonium sulfate was added to the obtained reaction solution, and the precipitated powder was collected by centrifugation, washed with pure water, and dried for 24 hours in a heating furnace with an internal temperature of 80°C to obtain a precursor of ferromagnetic powder. The obtained precursor of the ferromagnetic powder was placed in a heating furnace at an internal temperature of 1000° C. in an air atmosphere and subjected to a heat treatment for 4 hours. The heat-treated ferromagnetic powder precursor was placed in a 4 mol / L aqueous solution of sodium hydroxide (NaOH), and the liquid temperature was maintained at 70°C while stirring for 24 hours, thereby removing the impurity silicate compound from the heat-treated ferromagnetic powder precursor. Thereafter, the silicic acid compound was removed by centrifugation, and the ferromagnetic powder was collected and washed with pure water to obtain a ferromagnetic powder. The composition of the obtained ferromagnetic powder was confirmed by inductively coupled plasma-optical emission spectrometry (ICP-OES). The results showed that the powder was composed of Ga, Co, and Ti substituted ε-iron oxide (ε-Ga 0.28 Co 0.05 Ti 0.05 Fe 1.62In addition, X-ray diffraction analysis was performed under the same conditions as those described above for SrFe1, and it was confirmed from the peaks in the X-ray diffraction pattern that the obtained ferromagnetic powder had a single-phase ε-phase crystal structure (ε-iron oxide type crystal structure) that did not contain α-phase or γ-phase crystal structures. The average particle size of the obtained ε-iron oxide powder was 12 nm, and the activation volume was 746 nm. 3 , the anisotropy constant Ku is 1.2×10 5 J / m 3 , mass magnetization σs is 16A m 2 / kg.

[0107] The activation volume and anisotropy constant Ku of the above hexagonal strontium ferrite powder and ε-iron oxide powder were determined for each ferromagnetic powder by the method described above using a vibrating sample magnetometer (manufactured by Toei Kogyo Co., Ltd.). Moreover, the mass magnetization σs is a value measured at a magnetic field strength of 15 kOe using a vibrating sample magnetometer (manufactured by Toei Kogyo Co., Ltd.).

[0108] [Example 1] <Composition for forming magnetic layer> (Magnetic liquid) Ferromagnetic powder (see Table 1): 100.0 parts Oleic acid: 2.0 parts Vinyl chloride copolymer (Kaneka MR-104): 10.0 parts SO3Na group-containing polyurethane resin: 4.0 parts (Weight average molecular weight 70000, SO3Na group: 0.07meq / g) Additive A: 10.0 parts Methyl ethyl ketone: 150.0 parts Cyclohexanone: 150.0 parts (abrasive liquid) α-alumina (average particle size: 110 nm): 6.0 parts Vinyl chloride copolymer (Kaneka MR110): 0.7 parts Cyclohexanone: 20.0 parts (Protrusion forming agent liquid) Protrusion forming agent (see Table 1): 1.3 parts Methyl ethyl ketone: 9.0 parts Cyclohexanone: 6.0 parts (lubricant and hardener liquid) Stearic acid: 3.0 parts Stearic acid amide: 0.3 parts Butyl stearate: 6.0 parts Methyl ethyl ketone: 110.0 parts Cyclohexanone: 110.0 parts Polyisocyanate (Tosoh Corporation, Coronate (registered trademark) L): 3.0 parts

[0109] The above-mentioned additive A is a polymer synthesized by the method described in paragraphs 0115 to 0123 of JP2016-051493A.

[0110] <Composition for forming non-magnetic layer> Non-magnetic inorganic powder (α-iron oxide): 80.0 parts (Average particle size: 0.15 μm, average acicular ratio: 7, BET (Brunauer-Emmett-Teller) specific surface area: 52 m 2 / g) Carbon black (average particle size: 20 nm): 20.0 parts Electron beam curable vinyl chloride copolymer: 13.0 parts Electron beam curing polyurethane resin: 6.0 parts Phenylphosphonic acid: 3.0 parts Cyclohexanone: 140.0 parts Methyl ethyl ketone: 170.0 parts Butyl stearate: 2.0 parts Stearic acid: 1.0 parts

[0111] <Composition for forming backcoat layer> Non-magnetic inorganic powder (α-iron oxide): 80.0 parts (Average particle size: 0.15 μm, average acicular ratio: 7, BET specific surface area: 52 m 2 / g) Carbon black (average particle size: 20 nm): 20.0 parts Carbon black (average particle size: 100 nm): 3.0 parts Vinyl chloride copolymer: 13.0 parts Sulfonic acid group-containing polyurethane resin: 6.0 parts Phenylphosphonic acid: 3.0 parts Cyclohexanone: 140.0 parts Methyl ethyl ketone: 170.0 parts Stearic acid: 3.0 parts Polyisocyanate (Tosoh Coronate): 5.0 parts Methyl ethyl ketone: 400.0 parts

[0112] <Preparation of compositions for forming each layer> The magnetic layer forming composition was prepared by the following method. The components of the magnetic liquid were mixed and diluted using an open kneader, and then dispersed in a horizontal bead mill disperser for 12 passes using zirconia (ZrO2) beads (hereinafter referred to as "Zr beads") with a particle size of 0.5 mm, with a bead filling rate of 80 volume %, a rotor tip peripheral speed of 10 m / sec, and a residence time of 2 minutes per pass. The components of the abrasive liquid were mixed, and then placed in a vertical sand mill disperser together with Zr beads having a particle size of 1 mm. The bead volume / (abrasive liquid volume+bead volume) was adjusted to 60% and subjected to a sand mill dispersion process for 180 minutes. The processed liquid was then removed and subjected to an ultrasonic dispersion filtration process using a flow-type ultrasonic dispersion filtration device. The magnetic liquid, abrasive liquid, protrusion-forming agent liquid, and lubricant and hardener liquid were introduced into a dissolver stirrer and stirred for 30 minutes at a peripheral speed of 10 m / sec. The mixture was then subjected to three passes at a flow rate of 7.5 kg / min using a flow-type ultrasonic disperser, and then filtered through a filter with a pore size of 1 μm to prepare a composition for forming a magnetic layer.

[0113] The composition for forming the nonmagnetic layer was prepared by the following method. The above components, except for the lubricants (butyl stearate and stearic acid), were kneaded and diluted using an open kneader, and then dispersed using a horizontal bead mill disperser.Then, the lubricants (butyl stearate and stearic acid) were added, and the mixture was stirred and mixed using a dissolver stirrer to prepare a nonmagnetic layer-forming composition.

[0114] The composition for forming the backcoat layer was prepared by the following method. The above components except lubricant (stearic acid), polyisocyanate and methyl ethyl ketone (400.0 parts) were kneaded and diluted by an open kneader, and then dispersed by a horizontal bead mill disperser. Then, lubricant (stearic acid), polyisocyanate and methyl ethyl ketone (400.0 parts) were added, and the mixture was stirred by a dissolver stirrer to prepare a backcoat layer forming composition.

[0115] <Production of magnetic tapes and magnetic tape cartridges> A non-magnetic layer forming composition was applied to a biaxially oriented polyethylene naphthalate support having a thickness of 4.2 μm so that the thickness after drying was 0.7 μm, and then it was irradiated with an electron beam at an acceleration voltage of 125 kV and an energy of 40 kGy. A magnetic layer forming composition was applied thereon so that the thickness after drying was 0.1 μm and dried, and a backcoat layer forming composition was further applied to the surface of the support opposite to the surface on which the non-magnetic layer and the magnetic layer were formed so that the thickness after drying was 0.3 μm, and then it was dried. The film was then calendered using a seven-stage calender roll consisting only of metal rolls at a calender speed of 80 m / min, a linear pressure of 294 kN / m, and the calender temperature shown in Table 1. It was then heat-treated for 36 hours in an atmosphere with a temperature of 70°C. After heat-treatment, the film was slit to a width of 1 / 2 inch, and the surface of the magnetic layer was cleaned using a tape cleaning device attached to a device having a delivery and take-up device with a nonwoven fabric and a razor blade pressed against the surface of the magnetic layer, to obtain a magnetic tape. A servo signal was recorded on the magnetic layer of the obtained magnetic tape by a commercially available servo writer, to obtain a magnetic tape having a data band, a servo band, and a guide band in an arrangement according to the LTO (Linear Tape-Open) Ultrium format, and a servo pattern (timing-based servo pattern) on the servo band in an arrangement and shape according to the LTO Ultrium format. The servo pattern thus formed is a servo pattern according to the descriptions in JIS (Japanese Industrial Standards) X6175:2006 and Standard ECMA-319 (June 2001). The total number of servo bands is 5, and the total number of data bands is 4. The magnetic tape (length 960 m) on which the servo signal was thus recorded was wound on a reel of a magnetic tape cartridge (LTO Ultrium 8 data cartridge). In this manner, the magnetic tape cartridge of Example 1 in which the magnetic tape was wound around the reel was produced.

[0116] [Examples 2 to 10, Comparative Examples 1 and 2] A magnetic tape and a magnetic tape cartridge were obtained in the same manner as in Example 1, except that the type of ferromagnetic powder, the type of protrusion-forming agent and / or the calender temperature were changed as shown in Table 1.

[0117] [Evaluation of driving stability] Using each of the magnetic tape cartridges of the examples and comparative examples, data was recorded and reproduced using a magnetic tape device configured as shown in Fig. 3. The recording and reproducing head mounted on the recording and reproducing head unit has 32 or more channels of reproducing elements (reproducing element width: 0.8 μm) and recording elements, and has servo signal reading elements on both sides. Data was recorded and reproduced by the following method, and the running stability during reproduction was evaluated. A magnetic tape cartridge is set in a magnetic tape device and the magnetic tape is loaded. Next, while performing servo tracking, the recording / playback head unit records pseudo-random data with a specific data pattern onto the magnetic tape. A constant tension is applied to the tape in the longitudinal direction during this process. At the same time as the data is recorded, the servo band intervals along the entire length of the tape are measured every 1m along the longitudinal direction and recorded in the cartridge memory. Next, the data recorded on the magnetic tape is played back by the recording / playback head unit while performing servo tracking. At the same time as playback, the servo band interval is measured, and based on the information recorded in the cartridge memory, the tension applied in the longitudinal direction of the tape is controlled so that the absolute value of the difference from the servo band interval at the time of recording at the same longitudinal position approaches zero. During playback, the servo band interval is measured and tension is controlled based on the measurement in real time continuously. The running stability was evaluated using as an index the standard deviation (hereinafter referred to as "σPES") of the read position PES (Position Error Signal) in the width direction based on the servo signal obtained by the servo signal reading element during the above reproduction. PES is calculated in the following manner: To calculate the PES, the dimensions of the servo pattern are required. The standard dimensions of the servo pattern differ depending on the generation of LTO. First, we use a magnetic force microscope or similar to measure the average distance AC between the four corresponding stripes of the A burst and the C burst, and the azimuth angle α of the servo pattern. The average time between five stripes corresponding to A burst and B burst over the length of one LPOS word is defined as a. The average time between four stripes corresponding to A burst and C burst over the length of one LPOS word is defined as b. In this case, the value defined by AC×(1 / 2-a / b) / (2×tan(α)) is the read position PES (Position Error Signal) in the width direction based on the servo signal obtained by the servo signal reading element over the length of one LPOS word. For the magnetic tape, the end wound on the reel of the magnetic tape cartridge is called the inner end, and the opposite end is called the outer end. The outer end is set to 0 m, and the standard deviation (σPES) of the PES obtained by the above method was calculated for a region in the tape longitudinal direction over a length of 30 m to 200 m. If σPES is less than 70 nm, it can be determined that the running stability is excellent.

[0118] [Magnetic tape evaluation] (1) Difference (S 0.1 -S 1.6 ) Using a TSA (Tape Spacing Analyzer, manufactured by Micro Physics), spacing measurements were carried out successively under pressures of 0.5 atm, 0.6 atm, 0.8 atm, 1.0 atm, 1.3 atm and 1.6 atm according to the following method. Five sample pieces of 5 cm in length were cut out from each of the magnetic tapes of the Examples and Comparative Examples, and each sample piece was washed with n-hexane by the method described above. A glass plate (glass plate (model number: WG10530) manufactured by Thorlabs, Inc.) provided in the TSA was placed on the magnetic layer surface of the magnetic tape (i.e., the above sample pieces) after the n-hexane washing, and a urethane hemisphere provided in the TSA was used as a pressing member, and this hemisphere was pressed against the backcoat layer surface of the magnetic tape at a pressure of 0.5 atm. In this state, white light was projected from a stroboscope provided in the TSA through the glass plate to focus on a certain area (150,000 to 200,000 μm) of the magnetic layer surface of the magnetic tape. 2) and the resulting reflected light was received by a CCD (Charge-Coupled Device) through an interference filter (a filter that selectively transmits light with a wavelength of 633 nm), obtaining an image of the interference fringes caused by the unevenness in this area. This image was divided into 300,000 points, and the distance (spacing) from the surface of the glass plate facing the magnetic tape to the surface of the magnetic layer of the magnetic tape at each point was determined and plotted as a histogram. The most frequent value of the histogram was determined as the spacing under a pressure of 0.5 atm. The same sample piece was pressed at further increased pressures, successively at 0.6 atm, 0.8 atm, 1.0 atm, 1.3 atm, and 1.6 atm, and the spacing measured at each pressure was determined by the above method. From the spacing values ​​obtained under each pressure, equations 1 and 2 were derived for each sample as shown above, and S was calculated using equation 2. 0.1 The S calculated for the five test pieces was 0.1 The arithmetic mean of the magnetic tape to be measured is 0.1 It was decided. In addition, the arithmetic mean of the spacing measurements obtained for the five test pieces under the pressure of 1.6 atm was calculated as the S 1.6 It was decided. And the S obtained in this way 0.1 and S. 1.6 The difference between the measured magnetic tape (S 0.1 -S 1.6 ) was sought. The values ​​obtained above are shown in Table 1.

[0119] (2) Tape thickness Ten tape samples (5 cm long) were cut out from any part of the magnetic tape taken out of each magnetic tape cartridge of the examples and comparative examples, and the tape samples were stacked and the thickness was measured. The thickness was measured using a digital thickness meter with a Millimar 1240 compact amplifier and a Millimar 1301 inductive probe manufactured by MARH. The measured thickness was divided by 10 to obtain the value (thickness per tape sample), which was taken as the tape thickness. The tape thickness of each magnetic tape was 5.3 μm.

[0120] The above results are shown in Table 1.

[0121] [Table 1]

[0122] From the results shown in Table 1, it can be confirmed that the magnetic tape of the embodiment is a magnetic tape that can exhibit excellent running stability in a magnetic tape device that controls the width direction of the magnetic tape by adjusting the tension applied in the longitudinal direction of the magnetic tape. [Industrial Applicability]

[0123] One aspect of the present invention is useful in various data storage technical fields.

Claims

1. A non-magnetic support and a magnetic layer containing ferromagnetic powder, the non-magnetic support comprises at least one material selected from the group consisting of polyethylene terephthalate and polyethylene naphthalate; The spacing S required on the surface of the magnetic layer after washing with n-hexane 0.1 and spacing S 1.6 The difference between 0.1 -S 1.6 , is less than or equal to 32 nm; The spacing S 0.1 is a value calculated as the spacing under a pressure of 0.1 atm from a relational equation between the pressure and the spacing obtained by measuring the spacing by optical interference method under a plurality of different pressures after washing the surface of the magnetic layer with n-hexane, The spacing S 1.6 is the spacing measured by optical interferometry under a pressure of 1.6 atm on the surface of the magnetic layer after washing with n-hexane.

2. 2. The magnetic tape of claim 1, wherein the difference is 30 nm or less.

3. 3. The magnetic tape according to claim 1, wherein the difference is equal to or greater than 10 nm and equal to or less than 30 nm.

4. 4. The magnetic tape according to claim 1, wherein the magnetic layer contains inorganic oxide particles.

5. 5. The magnetic tape according to claim 4, wherein the inorganic oxide particles are composite particles of an inorganic oxide and a polymer.

6. 6. The magnetic tape according to claim 1, further comprising a non-magnetic layer containing non-magnetic powder between the non-magnetic support and the magnetic layer.

7. 7. The magnetic tape according to claim 1, further comprising a backcoat layer containing nonmagnetic powder on the surface of the nonmagnetic support opposite to the surface having the magnetic layer.

8. 8. The magnetic tape according to claim 1, wherein the tape thickness is 5.3 μm or less.

9. A magnetic tape cartridge comprising the magnetic tape according to any one of claims 1 to 8.

10. A magnetic tape device comprising the magnetic tape cartridge according to claim 9.

Citation Information

Patent Citations

  • Thickness evaluation method of lubricant layer in magnetic tape surface layer

    JP2010192065A

  • Magnetic recording medium

    JP2012043495A

  • Magnetic tape device and head tracking servo method

    JP2018106789A

  • Magnetic recording medium and magnetic recording and reproducing device

    JP2019175537A

  • magnetic recording media

    JP6590104B1