SUBSTRATE PROCESSING METHOD AND SUBSTRATE PROCESSING APPARATUS

The substrate processing method addresses shape abnormalities in high aspect ratio contact holes by forming a protective film during etching and using subsequent steps to control pattern shape, achieving precise and efficient semiconductor feature formation.

JP7566099B2Active Publication Date: 2024-10-11TOKYO ELECTRON LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023136150
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-08-24
Publication Date
2024-10-11
Estimated Expiration
2039-06-28

AI Technical Summary

Technical Problem

Conventional plasma etching methods struggle to control shape abnormalities, such as bowing, during the formation of high aspect ratio contact holes in semiconductor manufacturing.

Method used

A substrate processing method that involves forming a protective film on the sidewalls of a pattern using sputtered products from a silicon-containing film while etching, combined with subsequent steps to control the shape, including mask lamination and blockage removal, to maintain pattern integrity.

Benefits of technology

The method effectively suppresses bowing and controls the shape of patterns on substrates, enabling the formation of high aspect ratio features with improved precision and reduced blockages.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007566099000001
    Figure 0007566099000001
  • Figure 0007566099000002
    Figure 0007566099000002
  • Figure 0007566099000003
    Figure 0007566099000003
Patent Text Reader

Abstract

To control a pattern shape formed on a substrate by etching.SOLUTION: A substrate processing method includes a step of providing a substrate and a first step. In the step of providing the substrate, a first film and a second film formed on the first film and having a pattern formed on the first film is provided. In the first step, a first processing gas is turned into plasma and the first film is etched at the same time as the sputtering of the second film, and a protective film is formed on the side wall of the first film with a product generated by the sputtering.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The following disclosure relates to a substrate processing method and a substrate processing apparatus. [Background technology]

[0002] Conventionally, in the manufacturing process of semiconductor devices, plasma etching has been used to form cylinder holes, contact holes, etc. In recent years, there has been a demand to suppress shape abnormalities such as bowing in the formation of high aspect ratio contact holes (HARC (High Aspect Ratio Contact)) and the like.

[0003] For example, a method has been proposed in which a substrate has an organic film, a silicon-containing film, and a pattern mask stacked in that order from the bottom, a recess is formed in the organic film, and then a protective film is formed on the inner wall surface of the recess by sputtering the silicon-containing film (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2009-49141 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present disclosure provides a technique that can control the shape of a pattern formed on a substrate by etching. [Means for solving the problem]

[0006] A substrate processing apparatus and a substrate processing method according to an embodiment of the present disclosure include a step of providing a substrate, and a first step. In the step of providing a substrate, a substrate having a first film and a second film formed on the first film and having an opening formed therein is provided. In the first step, a first processing gas is turned into plasma to sputter the second film and simultaneously etch the first film, while a protective film is formed on a sidewall of the first film by a product generated by the sputtering. Effect of the Invention

[0007] According to the present disclosure, it is possible to control the shape of a pattern formed on a substrate by etching. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a flowchart showing an example of a flow of a substrate processing method according to an embodiment. [Diagram 2] FIG. 2 is a diagram for explaining an example of a laminated structure processed by the substrate processing method according to an embodiment. [Diagram 3] FIG. 3 is a view for explaining a protective film forming step of the substrate processing method according to the embodiment. [Figure 4] FIG. 4 is a view for explaining an etching process of a substrate processing method according to an embodiment. [Figure 5A] FIG. 5A is a view for explaining a mask stacking step of the substrate processing method according to one embodiment. [Figure 5B] FIG. 5B is a view for further illustrating the mask stacking step of the substrate processing method according to the embodiment. [Figure 6A] FIG. 6A is a view for explaining an obstruction removal step in the substrate processing method according to one embodiment. [Figure 6B] FIG. 6B is a view for further illustrating the obstruction removal step of the substrate processing method according to the embodiment. [Figure 7A] FIG. 7A is a diagram for explaining an example of the flow of the process in FIG. [Figure 7B]FIG. 7B is a diagram for explaining another example of the processing flow of FIG. [Figure 8] FIG. 8 is a flowchart showing a cycle example 1 of a substrate processing method according to an embodiment. [Figure 9] FIG. 9 is a flowchart showing a second cycle example of a substrate processing method according to an embodiment of the present invention. [Figure 10] FIG. 10 is a flowchart showing a cycle example 3 of the substrate processing method according to the embodiment. [Figure 11] FIG. 11 is a flow chart showing an example of a combination of cycles of a substrate processing method according to an embodiment. [Figure 12] FIG. 12 is a diagram for explaining effects obtained by the substrate processing method according to an embodiment of the present invention. [Figure 13] FIG. 13 is a diagram for explaining conditions used for determining whether or not processing needs to be performed in the substrate processing method according to an embodiment. [Figure 14] FIG. 14 is a diagram showing an example of a configuration of a substrate processing apparatus for implementing a substrate processing method according to an embodiment of the present invention. [Figure 15A] FIG. 15A is a diagram for explaining a stacked structure formed in a manufacturing process of a semiconductor device. [Figure 15B] FIG. 15B is a diagram for explaining a photoresist pattern formed in the manufacturing process of the semiconductor device. [Figure 15C] FIG. 15C is a diagram for explaining a pattern of a silicon-containing film formed in a manufacturing process of a semiconductor device. [Figure 15D] FIG. 15D is a diagram for explaining a mask pattern formed in a manufacturing process of a semiconductor device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the disclosed embodiments will be described in detail with reference to the drawings. Note that the present embodiments are not limited to the above. In addition, the embodiments can be appropriately combined as long as the processing contents are not contradictory.

[0010] (An example of a shape defect that occurs during the manufacturing process of a semiconductor device) Before describing the embodiment, a shape abnormality occurring in the manufacturing process of a semiconductor device will be described. Fig. 15A is a diagram for explaining a stacked structure formed in the manufacturing process of a semiconductor device. Figs. 15B, 15C, and 15D are diagrams for explaining a photoresist pattern, a silicon-containing film pattern, and a mask pattern, respectively, formed in the manufacturing process of a semiconductor device.

[0011] First, as shown in FIG. 15A, for example, an organic film 12, a silicon-containing film 13, and a photoresist (PR) 14, which are films to be etched, are laminated on an insulating film 11. In the example of FIG. 15A, the insulating film 11 is, for example, a SiO2 film. The organic film 12 is, for example, a film containing carbon as a main component. The organic film 12 is, for example, an amorphous carbon film (ACL: Amorphous Carbon Layer). The silicon-containing film 13 is an inorganic film containing silicon as a main component. The silicon-containing film 13 is, for example, a SiO2 (silicon dioxide) film, a SiN (silicon nitride) film, a SiON (silicon oxynitride) film, a Poly-Si (polycrystalline silicon) film, or a SiCN (silicon carbonitride) film. The silicon-containing film 13 may be formed of a material that functions as an anti-reflection film (Arc: Anti-Reflection Coating) in a lithography process.

[0012] After the laminated structure shown in FIG. 15A is formed, a pattern is formed in the photoresist 14 by photolithography as shown in FIG. 15B. The photoresist 14 may be processed by extreme ultraviolet lithography (EUVL). Next, etching gas such as CF4 is turned into plasma from above the pattern of the photoresist 14 to perform etching. The silicon-containing film 13 is removed along the pattern of the photoresist 14, so that the pattern shown in FIG. 15C is formed in the silicon-containing film 13. Furthermore, O2 gas, H2 gas, N2 gas, or a mixed gas of H2 gas and N2 gas is turned into plasma from above the pattern formed in the silicon-containing film 13 to etch the organic film 12. As shown in FIG. 15D, the mask pattern formed in the organic film 12 becomes a mask pattern when etching the insulating film 11 below the organic film 12.

[0013] During etching of the organic film 12, the organic film 12 is isotropically etched by oxygen radicals, and a bowing 20 is formed in which the vertical cross section of the mask pattern expands in the horizontal direction, as shown in Fig. 15D. When the insulating film 11 is etched using the mask pattern with the bowing 20 formed therein, the shape of the organic film 12 is transferred to the insulating film 11, and the shape of the hole formed in the insulating film 11 deteriorates.

[0014] (Embodiment) Therefore, in the embodiment described below, when etching an organic film using a silicon-containing film as a hard mask, a product (deposit) generated by sputtering the silicon-containing film is used as a protective film for the organic film. In the substrate processing method according to the first embodiment, the region on which the protective film is formed is, for example, a region of a pattern to be formed on the organic film having an aspect ratio of at least 5, for example, an aspect ratio of about 5 to 7. In addition, in the substrate processing method according to the first embodiment, a shape of a pattern formed on a substrate by etching is controlled by combining a plurality of processing steps. In one of the steps, for example, sidewall protection of the pattern is realized by a sputter product generated by sputtering.

[0015] In the substrate processing method according to an embodiment, a layered structure S (see FIG. 2) in which an insulating film 31, an organic film 32, and a silicon-containing film 33 are layered in this order on a substrate is formed in the organic film 32 with a pattern for etching the insulating film 31. FIG. 2 is a diagram for explaining an example of a layered structure processed by the substrate processing method according to an embodiment.

[0016] The insulating film 31 is, for example, a SiO2 film. A predetermined pattern is formed in the insulating film 31 by performing etching from above the pattern formed in the organic film 32. The pattern formed in the insulating film 31 becomes a cylinder hole, a contact hole, etc. of a semiconductor device.

[0017] The organic film 32 is, for example, a film containing carbon as a main component. The organic film 32 is, for example, an amorphous carbon film. The substrate processing method according to this embodiment mainly controls the shape of a pattern to be formed in the organic film 32.

[0018] The silicon-containing film 33 is, for example, a SiO2 film, a SiN film, a SiON film, a Poly-Si film, or a SiCN film. The silicon-containing film 33 may be made of a material that functions as an anti-reflective film in a lithography process. The silicon-containing film 33 functions as a hard mask when etching the organic film 32. A predetermined pattern is formed in the silicon-containing film 33. Hereinafter, the pattern formed in the silicon-containing film 33 will be referred to as an "opening."

[0019] The substrate processing method according to one embodiment controls the pattern formed in the organic film 32 by combining the following steps (1) to (4). (1) Protective film formation process (2) Etching process (3) Mask stacking process (4) Obstruction removal process

[0020] (Protective film formation process) In the protective film forming process, the process gas is turned into plasma, and the organic film 32 is etched while sputtering the silicon-containing film 33. The sputtering product of the silicon-containing film 33 generated by sputtering is deposited on the sidewall of a recess formed in the organic film 32 to form a protective film 40. The process gas used in the protective film forming process is an example of a first process gas. The protective film forming process is also an example of a first process.

[0021] FIG. 3 is a diagram for explaining a protective film forming step of a substrate processing method according to an embodiment. It is assumed that the protective film forming step is performed on the laminated structure S shown in FIG. 2. In the protective film forming step, a processing gas containing, for example, hydrogen (H2) is turned into plasma and the laminated structure S is exposed to the plasma. The silicon-containing film 33 is sputtered by being exposed to the plasma of H2, and the sputtering product scattered by the sputtering is deposited on the side wall of the recess of the organic film 32. Therefore, the laminated structure S in FIG. 3 includes the silicon-containing film 33 and the protective film 40 deposited on the side wall of the recess of the organic film 32. In the protective film forming step, the formation of the protective film 40 by sputtering the silicon-containing film 33 and the etching of the recess of the organic film 32 proceed simultaneously by the plasma of the processing gas. The processing gas may be H2 alone or a mixed gas of N2 (nitrogen) gas and H2 gas.

[0022] (Etching process) FIG. 4 is a diagram for explaining an etching process of a substrate processing method according to an embodiment. In the etching process, a processing gas is turned into plasma, and the organic film 32 is etched in the depth direction using the silicon-containing film 33 as a mask. The processing gas used in the etching process is an example of a second processing gas. The etching process is an example of a second process. The organic film 32 is etched using a mixed gas of O2 (oxygen) gas and COS (carbonyl sulfide) gas. Cl2 (chlorine), HBr (hydrogen bromide), etc. may be added to the processing gas. The processing gas is prepared so as to mainly etch the organic film 32. By performing the etching process, the silicon-containing film 33, which is a hard mask, is gradually removed, and recesses corresponding to the openings of the silicon-containing film 33 are formed in the organic film 32, and the recesses gradually become deeper.

[0023] (Mask stacking process) In the mask lamination step, the thickness of the silicon-containing film 33 is increased, for example, by anisotropic film formation. The mask lamination step is an example of the third step. FIGS. 5A and 5B are diagrams for explaining the mask lamination step of the substrate processing method according to one embodiment. As shown in FIG. 5A, when the protective film formation in the protective film formation step or the etching in the etching step is performed, the thickness of the silicon-containing film 33 gradually decreases. When the aspect ratio of the pattern formed in the organic film 32 is high, the silicon-containing film 33, which is a hard mask, may disappear before the bottom of the pattern reaches the insulating film 31. Therefore, in the mask lamination step, a film is formed from above the silicon-containing film 33 using plasma of a third processing gas. The film formation conditions are set to be anisotropic. That is, the conditions are set so that the film is mainly formed on the top of the silicon-containing film 33 and the opening is not blocked (see FIG. 5B).

[0024] The third process gas in the mask lamination process may be, for example, a mixed gas of a silicon halide gas such as SiCl4 or SiF4, a rare gas such as argon (Ar), and O2. The third process gas is turned into plasma, and the laminated structure S is exposed to the plasma. The film formation method is not particularly limited, and may be chemical vapor deposition (CVD), physical vapor deposition (PVD), atomic layer deposition (ALD), direct current superposition (DCS), or the like. The composition of the film formed in the mask lamination process does not need to be the same as that of the silicon-containing film 33. The film formed in the mask lamination process may be, for example, a silicon-containing film having a different composition from that of the silicon-containing film 33. The film formed in the mask lamination process may be a material that can obtain a high selectivity with the organic film 32, and may not be a silicon-containing film.

[0025] (Occlusion removal process) 6A and 6B are diagrams for explaining an obstruction removal step of a substrate processing method according to an embodiment. In the obstruction removal step, obstructions blocking the opening and / or the upper part of the pattern generated in any one of the protective film formation step, the etching step, and the mask stacking step are removed by a processing gas containing fluorine (F). The processing gas used in the obstruction removal step is an example of a fourth processing gas. The obstruction removal step is also an example of a fourth step. As shown in FIG. 6A, in the process of forming a pattern on a stacked structure S, products (D in FIG. 6A(1)) generated by etching may adhere to the side walls of the opening, gradually blocking the opening. Alternatively, products (D' in FIG. 6A(2)) may grow horizontally in the mask stacking, gradually blocking the opening or the upper part of the pattern. Therefore, in the obstruction removal step, obstructions (products) blocking the opening or the pattern are removed by plasma of a fluorine-containing gas. By removing a part of the product D or the product D', the opening dimension of the silicon-containing film 33 is restored (FIGS. 6B(1) and (2)), and the processing gas can reach the bottom of the pattern in the subsequent process (e.g., etching process). The processing gas used in the obstruction removal process may be a mixed gas of a fluorine-containing gas such as CHF3 or CF4 and a rare gas such as N2 gas or argon (Ar) gas.

[0026] Next, a substrate processing method according to an embodiment will be described with reference to Fig. 1 and Fig. 7A. Fig. 1 is a flow chart showing an example of the flow of the substrate processing method according to an embodiment. Fig. 7A is a diagram for explaining an example of the process flow of Fig. 1.

[0027] First, a stacked structure S is prepared (step S100, (1) in FIG. 7A). Next, it is determined whether the stacked structure S satisfies condition A (step S101). Condition A is, for example, that the thickness of the silicon-containing film 33 on the organic film 32 is equal to or greater than a predetermined value. Usually, in the first cycle, the stacked structure S satisfies condition A (step S101, Yes), and the process proceeds to step S103 without executing the mask stacking process. On the other hand, in the second or subsequent cycles, if it is determined that condition A is not satisfied (step S101, No), the mask stacking process is executed (step S102).

[0028] In step S103, it is determined whether or not the stacked structure S satisfies condition B. Condition B is, for example, that the aspect ratio of the pattern formed in the organic film 32 reaches a predetermined value α. The predetermined value α is, for example, 5. In addition, condition B is, for example, that a protective film 40 (see FIG. 3) is formed on the pattern formed in the organic film 32.

[0029] When it is determined that the condition B is not satisfied (step S103, No), the protective film forming process is executed (step S104, (2) of FIG. 7A). For example, when no pattern is formed on the organic film 32, it is determined that the condition B is not satisfied. By executing the protective film forming process, the etching of the organic film 32 progresses, and at the same time, the sputtering product of the silicon-containing film 33 generated by sputtering the silicon-containing film 33 is deposited on the sidewall of the pattern (recess) formed on the organic film 32 to form the protective film 40. When step S104 is completed, the process returns to step S101 and is repeated. At this time, when it is determined that the film thickness of the silicon-containing film 33 is reduced by executing the protective film forming process and the condition A is not satisfied (step S101, No), the mask stacking process is executed (step S102).

[0030] On the other hand, if it is determined that condition B is satisfied (Yes at step S103), the process proceeds to step S105. For example, if the aspect ratio of the pattern formed in the organic film 32 is 6, it is determined that condition B is satisfied. Also, for example, if the aspect ratio of the pattern formed in the organic film 32 reaches 5 by performing the protective film formation process several times, it is determined that condition B is satisfied. If it is determined that condition B is satisfied, the process proceeds to step S105.

[0031] In one embodiment, once condition B is satisfied, a protective film may not be formed in the subsequent steps. In this case, after proceeding to step S105 once, the determination in step S103 is YES again. However, if the protective film 40 is scraped off by repeatedly executing step S106 and condition B is no longer satisfied (step S103, No), a protective film forming step may be executed (step S104).

[0032] In step S105, it is determined whether the stacked structure S satisfies condition C. For example, condition C is that the opening dimension of the silicon-containing film 33 is equal to or larger than a predetermined dimension. If it is determined that condition C is not satisfied (step S105, No), an obstruction removal process is executed (step S106). When step S106 is completed, the process returns to step S101 and is repeated. On the other hand, if it is determined that condition C is satisfied (step S105, Yes), the process proceeds to the next step S107.

[0033] In step S107, it is determined whether the stacked structure S satisfies condition D. For example, the condition D is that the aspect ratio of the pattern formed in the organic film 32 is equal to or greater than a predetermined value β different from α. The predetermined value β is, for example, 20 to 30. If it is determined that the condition D is not satisfied (step S107, No), an etching process is performed (step S108, FIG. 7A (3)). When step S108 is completed, the process returns to step S101 and is repeated. At this time, the film thickness of the silicon-containing film 33 may be reduced by performing steps S104 and S108, and it may be determined that the condition A is not satisfied (step S101, No). In this case, a mask stacking process is performed (step S102, FIG. 7A (4)). Also, the opening dimension of the silicon-containing film 33 may be reduced by performing steps S102 and S108, and it may be determined that the condition C is not satisfied (step S106, No). In this case, the obstruction removal step is executed (step S106, (5) in FIG. 7A).

[0034] By repeatedly executing the above processes, if it is finally determined in step S107 that condition D is satisfied (Yes in step S107), the process ends.

[0035] FIG. 7B is a diagram for explaining another example of the process flow of FIG. 1. In FIG. 7B (1), the silicon-containing film 33 of the stacked structure S is considerably etched, but not below the predetermined value of condition A (step S101, Yes). Also, the aspect ratio of the mask pattern is less than the predetermined value β (step S107, No). Therefore, an etching process is performed to etch the mask pattern (step S108). As a result of the etching, the silicon-containing film 33 is etched and the film thickness becomes less than the predetermined value (step S101, No). Therefore, a mask stacking process is performed to stack masks (FIG. 7B (2)). When conditions A to D are satisfied, the process of the stacked structure S ends.

[0036] 1, the next process to be performed is selected according to the state of the laminated structure S after processing. Therefore, by appropriately setting conditions A to D for determining whether each process needs to be performed and selectively performing the protective film forming process, etching process, mask stacking process, and obstruction removal process, it is possible to perform processing suited to the state of the laminated structure S. Note that the determination of whether conditions A to D are satisfied is performed by setting in advance the number of times each process is to be performed until conditions A to D are satisfied, and the processing conditions to be applied to each process. For example, it is possible to determine whether conditions A to D are satisfied based on the number of times each process is performed.

[0037] In the example of Fig. 1, the protective film forming step, the etching step, the mask stacking step, and the obstruction removal step are performed after determining whether or not to perform each step according to conditions A to D. However, the flow of the substrate processing method according to this embodiment is not limited to the flow shown in Fig. 1. For example, among the protective film forming step, the etching step, the mask stacking step, and the obstruction removal step, the steps to be combined, and the order and number of times to perform the combined steps may be set in advance. For example, a cycle combining the protective film forming step, the etching step, the mask stacking step, and the obstruction removal step may be set in advance, and each cycle may be performed a predetermined number of times.

[0038] 8 is a flowchart showing cycle example 1 of a substrate processing method according to one embodiment. Cycle example 1 includes a protective film forming step (step S61) and a mask lamination step (step S62). In cycle example 1, first, a protective film is formed on a sidewall of the organic film 32 in the protective film forming step. Then, the mask height of the hard mask (silicon-containing film 33) that has been reduced by sputtering in the protective film forming step is restored in the mask lamination step. In addition, in FIGS. 8 to 10, "Pre-C" indicates the previous cycle, and "Post-C" indicates the subsequent cycle.

[0039] 9 is a flowchart showing cycle example 2 of the substrate processing method according to one embodiment. Cycle example 2 includes an etching step (step S71) and an obstruction removal step (step S72). In cycle example 2, first, a pattern of the organic film 32 is formed by etching the organic film 32. Then, products deposited on the side walls of the openings and the side walls of the upper part of the pattern by the etching step are removed by the obstruction removal step.

[0040] 10 is a flowchart showing cycle example 3 of the substrate processing method according to one embodiment. Cycle example 3 includes a mask stacking step (step S81), an etching step (step S82), and an obstruction removal step (step S83). In cycle example 3, first, the mask height of the hard mask (silicon-containing film 33) that has been reduced is restored. Then, the pattern of the organic film 32 is etched in the depth direction. Then, by-products deposited on the side walls of the openings and the side walls of the upper part of the pattern are removed by etching.

[0041] The shape of the pattern can be controlled by combining cycle examples 1 to 3 according to the depth of the pattern formed in the organic film 32. For example, cycle example 1 is performed when the organic film 32 has not yet been etched. Then, a protective film can be formed with the sputtering product of the silicon-containing film 33 while the organic film 32 is etched while suppressing bowing of the organic film 32. Furthermore, the top of the silicon-containing film 33 that has disappeared due to sputtering can be reinforced by the mask stacking process. Next, cycle example 2 is performed when the etching of the organic film 32 has progressed, for example, when the etching reaches a region where bowing is likely to occur. Then, since the area directly below the silicon-containing film 33 where bowing is likely to occur is protected by the protective film 40, etching can be progressed while suppressing bowing of the organic film 32. Furthermore, the etching product deposited on the sidewall of the opening and the sidewall of the upper part of the pattern can be removed by the blockage removal process. When the etching of the organic film 32 further progresses, the hard mask is reduced again, so cycle example 3 is performed. With cycle example 3, etching can be progressed after stacking a hard mask, and blockage of the opening at the top of the pattern can be suppressed.

[0042] In this manner, the shape of the pattern can be controlled by combining a cycle that combines a protective film formation process, an etching process, a mask stacking process, and an obstruction removal process in accordance with the state of the pattern formed in the stacked structure S, for example, the depth of the pattern.

[0043] Fig. 11 is a flow chart showing an example of cycle combination of a substrate processing method according to an embodiment. In the example of Fig. 11, after the above-mentioned cycle example 1 is executed a predetermined number of times, for example, five times, cycle example 2 is executed a predetermined number of times, for example, three times, and cycle example 3 is executed a predetermined number of times, for example, four times. In addition, the processing conditions of cycle example 3 are changed. For example, cycle example 3 is executed four times, and among them, the change is made between the first three times and the last one.

[0044] First, when the process starts, cycle example 1 is executed (step S901). Then, it is determined whether cycle example 1 has been executed a predetermined number of times (step S902). If it is determined that cycle example 1 has not been executed a predetermined number of times (step S902, No), the process returns to step S901 and cycle example 1 is repeated. On the other hand, if it is determined that cycle example 1 has been executed a predetermined number of times (step S902, Yes), the process proceeds to step S903 and cycle example 2 is executed. Then, it is determined whether cycle example 2 has been executed a predetermined number of times (step S904). If it is determined that cycle example 2 has not been executed a predetermined number of times (step S904, No), the process returns to step S903 and cycle example 2 is repeated. On the other hand, if it is determined that cycle example 2 has been executed a predetermined number of times (step S904, Yes), the process proceeds to step S905 and cycle example 3 is executed. Here, cycle example 3 in step S905 is executed under process condition 1. For example, under process condition 1, the process time of the mask stacking step is set to 10 seconds. Next, it is determined whether cycle example 3 based on process condition 1 has been executed a predetermined number of times (step S906). If it is determined that the cycle has not been performed the predetermined number of times (step S906, No), the process returns to step S905 to repeat cycle example 3. On the other hand, if it is determined that the cycle has been performed the predetermined number of times (step S906, Yes), the process proceeds to step S907 to perform cycle example 3. Cycle example 3 in step S907 is performed under process condition 2. For example, under process condition 2, the processing time for the mask stacking step is set to 20 seconds. Then, it is determined whether cycle example 3 under process condition 2 has been performed the predetermined number of times (step S908). If it is determined that the cycle has not been performed the predetermined number of times (step S908, No), the process returns to step S907 to repeat cycle example 3. On the other hand, if it is determined that the cycle has been performed the predetermined number of times (step S908, Yes), the process ends.

[0045] In this manner, the substrate processing method according to the embodiment changes the process and processing conditions to be performed depending on the processing state of the pattern formed in the laminate structure S, for example, the progress state of etching. In addition, the processing is simplified by repeatedly executing a cycle in which multiple processes are combined.

[0046] (Verification results) 12 is a diagram for explaining the effect obtained by the substrate processing method according to one embodiment. In FIG. 12, (A) shows a state in which a pattern is formed in the silicon-containing film 33 on the organic film 32 (corresponding to FIG. 2). In (A), the positions of the insulating film 31, the organic film 32, and the silicon-containing film 33 are indicated by arrows. Also, (B) shows the state of the processed object (Comparative Example) when an etching process is performed without forming a protective film (40 in FIG. 3) on the laminated structure shown in (A). Also, (C) shows the state of the processed object (Example) when a pattern of an organic film is formed on the laminated structure shown in (A) by the substrate processing method according to the above embodiment.

[0047] Each of the objects to be processed was formed to include an insulating film 31 (film to be etched), an organic film 32 (mask) formed on the insulating film 31, and a silicon-containing film 33 (hard mask) formed on the organic film 32. After that, an opening was formed in the silicon-containing film 33 as shown in Fig. 12(A). In (A), the organic film 32 has also been slightly removed by the effect of etching.

[0048] First, in Comparative Example (B), a mixed gas of O2 gas and COS gas was supplied into the chamber at a flow rate of 250 / 50, and the organic film 32 was etched using the silicon-containing film 33 as a hard mask. The pressure in the chamber was set to 20 mTorr, and the voltages of the upper electrode and the lower electrode were set to 1400 W and 500 W. The frequencies of the upper electrode and the lower electrode were set to 27 MHz and 13 MHz, respectively. The temperatures (T / W / B) of the top, sidewall, and bottom of the chamber were set to 120° C., 100° C., and 10° C., respectively. The etching process was performed once, with one etching process lasting 300 seconds.

[0049] In Example (C), cycle examples 1 to 3 were performed in the combination shown in Fig. 11. Specifically, cycle example 1 was performed five times, cycle example 2 was performed three times, and cycle example 3 was performed three times with a processing time of 10 seconds for the obstruction removal step and once with a processing time of 20 seconds for the mask stacking step, in that order.

[0050] The processing conditions for each of the protective film forming step, the etching step, the mask stacking step and the obstruction removing step are as follows. Protective film formation process: Chamber pressure: 20mTorr Upper and lower electrode voltage 0W+900W H2 gas flow rate: 250sccm Temperature inside the chamber: T / W / B=120℃ / 100℃ / 10℃ Processing time: 120 seconds Etching process: Chamber pressure: 20mTorr Processing gas flow rate: O2 / CO2 / =250sccm / 50sccm Temperature inside the chamber: T / W / B=120℃ / 100℃ / 10℃ Processing time: 100 seconds Mask stacking process: Chamber pressure: 20mTorr Upper and lower electrode voltage: 800W+0W Processing gas flow rate: Ar / O2 / SiCl4=500sccm / 100sccm / 20sccm Temperature inside the chamber: T / W / B=120℃ / 100℃ / 10℃ Obstruction removal process: Chamber pressure: 30mTorr Upper and lower electrode voltage: 300W+140W Processing gas flow rate: CHF3 / CF4 / N2=300sccm / 100sccm / 150sccm Temperature inside the chamber: T / W / B=120℃ / 100℃ / 10℃ Processing time: 30 seconds

[0051] The processed object shown in Fig. 12B was obtained by the processing of the comparative example. As can be seen from Fig. 12B, in the comparative example, bowing occurs in the upper part of the organic film 32 (the part shown by the dotted rectangle). As a result, the pattern formed in the organic film 32 has a shape that tapers from top to bottom as a whole, and the opening dimension at the bottom of the pattern is somewhat narrow (about 78 nm). The vertical dimension of the pattern is about 2500 nm.

[0052] In contrast, in the embodiment (FIG. 12C), a protective film 40 was first formed by Cycle Example 1, and the pattern shown on the left side of (C) was formed on the organic film 32 (see the left side of FIG. 12C). After the aspect ratio reached about 5, Cycle Examples 2 and 3 were performed to complete the pattern of the organic film 32 (see the right side of FIG. 12C).

[0053] 12C, in the embodiment, almost no bowing occurs in the upper part of the organic film 32, and therefore the lateral spread is significantly reduced compared to the comparative example (area indicated by a dotted rectangle). Specifically, the lateral dimension of the bowing, which was about 170 nm in the comparative example, is improved to about 105 nm in the embodiment. In addition, the pattern formed in the organic film 32 has a suppressed top-to-bottom taper overall, and the opening dimension at the bottom of the pattern is improved (about 87 nm) compared to the comparative example.

[0054] In the protective film forming process of the above embodiment, hydrogen (H2) gas is used as the processing gas. However, processing gases other than hydrogen gas can also be used as the processing gas in the protective film forming process as long as the protective film forming speed is faster than the speed at which bowing occurs after etching progresses.

[0055] (An example of an area where a protective film is formed) The inventors also studied conditions used to determine whether or not a protective film forming step needs to be performed. Fig. 13 is a diagram for explaining conditions used to determine whether or not a process needs to be performed in a substrate processing method according to an embodiment. Condition B for determining whether or not a protective film forming step needs to be performed will be explained with reference to Fig. 13.

[0056] The six patterns (A) to (F) shown in FIG. 13 each show an example of the following state. (A) State 1 immediately after a pattern is formed on the silicon-containing film 33 of the stacked structure S (B) State 2 after the protective film formation process was performed for 30 seconds on the pattern in state 1 (C) State 3 after the etching process was performed for 300 seconds on the pattern in state 2 (D) State 4 after the protective film formation process was performed for 120 seconds on the pattern in state 1 (E) State 5 after the etching process was performed for 300 seconds on the pattern in state 4 (F) State 6 after the protective film formation process was performed for 600 seconds on the pattern in state 1 In the example of FIG. 13, the process conditions for the protective film forming step and the etching step are as follows: Protective film formation process: Chamber pressure: 20mTorr Upper and lower electrode voltage: 0W+900W Processing gas flow rate: H2=250 Temperature inside the chamber: T / W / B=120℃ / 100℃ / 10℃ Etching process: Chamber pressure: 20mTorr Upper and lower electrode voltage: 1400W+500W Processing gas flow rate: O2 / CO2=250sccm / 50sccm Temperature inside the chamber: T / W / B=120℃ / 100℃ / 10℃

[0057] In state 1 shown in (A) of Fig. 13, an opening tapering from the top to the bottom is formed in silicon-containing film 33 of stacked structure S. The thickness of silicon-containing film 33 shown in the example of Fig. 13 is about 215 nanometers. When the protective film forming step is performed for 30 seconds on stacked structure S under the above-mentioned processing conditions, organic film 32 is etched and protective film 40 is formed on the side wall of the opening formed by etching, as shown in (B).

[0058] When an etching process is performed for 300 seconds on stacked structure S in state 2, bowing occurs that spreads laterally from directly below the opening portion formed in organic film 32 in state 2, and organic film 32 is removed into the shape shown in (C). In state 3, bowing does not occur in the opening formed in organic film 32 at the position where protective film 40 is formed (location indicated by A1 in FIG. 13), but bowing occurs directly below protective film 40.

[0059] When the processing time of the protective film forming step is extended from 30 seconds to 120 seconds, the depth of the opening formed in the organic film 32 increases, and accordingly, the region in which the protective film 40 is formed becomes wider in the depth direction ((D) of FIG. 13). In state 4 shown in (D), the protective film 40 is formed to a depth of about 130 nanometers from the top of the organic film 32 (see the portion indicated by A2 in FIG. 13). When the etching step is performed for 300 seconds under the above processing conditions for the stacked structure S in state 4, as shown in (E), the position where bowing occurs moves downward compared to the example in (C), and the amount of bowing is reduced. In this way, it can be seen that the position and amount of bowing can be controlled by forming the protective film 40. However, in the example in (E), as a result of the etching step, the silicon-containing film 33 that plays the role of a mask is scraped off, and the opening is blocked by deposits adhering to the top.

[0060] Furthermore, as shown in (F), when the protective film forming step is performed for 600 seconds under the above processing conditions on the stacked structure S in state 1, the protective film 40 formed on the organic film 32 reaches a depth of about 380 nanometers in the opening. However, as the processing time of the protective film forming step increases, the amount of silicon-containing film 33 that is removed also increases. In the example shown in (F), the mask portion of the silicon-containing film 33 is removed in the thickness direction, and the shape is distorted and the surface is rough.

[0061] Thus, when the aspect ratio of the pattern formed in the organic film 32 is large, the mask pattern of the silicon-containing film 33 disappears and the opening is blocked by simply repeating the protective film forming process and the etching process. On the other hand, the inventors have found, as a result of the above experiments, that when the pattern formed in the organic film 32 has a diameter of, for example, about 100 nanometers and a depth of 2000 to 3000 nanometers, bowing can be effectively suppressed by forming a protective film on the top of the opening. For example, in the case of an opening with a diameter of 100 nanometers, bowing can be significantly reduced by forming the protective film 40 in a region about 500 nanometers from the top. In addition, bowing can be significantly reduced by forming the protective film 40 in a region with an aspect ratio of about 6.7. From this, the inventors have concluded that the pattern shape can be improved by forming the protective film 40 to an aspect ratio of about 5 to 7.

[0062] (Configuration example of substrate processing apparatus) 14 is a cross-sectional view showing a schematic configuration of a substrate processing apparatus 100 according to one embodiment. The substrate processing apparatus 100 includes a processing chamber 102 made of metal (for example, aluminum) and formed in a tubular (for example, cylindrical) shape.

[0063] A mounting table 110 for mounting the wafer W thereon is provided at the bottom of the processing chamber 102. The mounting table 110 is formed into a generally columnar (e.g., cylindrical) shape from aluminum or the like. Although not shown, the mounting table 110 can be provided with various functions as necessary, such as an electrostatic chuck that attracts and holds the wafer W by electrostatic force, and a temperature adjustment mechanism such as a heater and a coolant flow path. In the case of an etching apparatus, a bias high frequency is applied to the mounting table 110 to attract ions to the wafer W.

[0064] A plate-shaped dielectric 104 made of, for example, quartz glass or ceramic is provided on the ceiling of the processing chamber 102 so as to face the mounting table 110. Specifically, the plate-shaped dielectric 104 is formed, for example, in a disk shape, and is attached airtightly so as to cover an opening formed in the ceiling of the processing chamber 102.

[0065] The processing chamber 102 is provided with a gas supply unit 120 that supplies a processing gas for processing the wafer W. A gas inlet 121 is formed in a sidewall of the processing chamber 102, and a gas supply source 122 is connected to the gas inlet 121 via a gas supply pipe 123. A flow rate controller, such as a mass flow controller (MFC) 124 for controlling the flow rate of the processing gas, and an opening / closing valve 126 are provided in the gas supply pipe 123. According to the gas supply unit 120, the processing gas from the gas supply source 122 is controlled to a predetermined flow rate by the mass flow controller 124 and supplied into the processing chamber 102 from the gas inlet 121.

[0066] In FIG. 14, for the sake of simplicity, the gas supply unit 120 is represented by a single gas line system, but the gas supply unit 120 is not limited to supplying a single type of processing gas, and may supply multiple types of gas as processing gas. In this case, multiple gas supply sources may be provided to configure multiple gas lines, and each gas line may be provided with a mass flow controller. In addition, FIG. 14 shows an example in which the gas supply unit 120 is configured to supply gas from the side wall of the processing chamber 102, but this is not necessarily limited to this. For example, the gas may be configured to supply gas from the ceiling of the processing chamber 102. In this case, a gas inlet may be formed, for example, in the center of the plate-shaped dielectric 104, and gas may be supplied from there.

[0067] For example, in etching an oxide film, a halogen-based gas containing Cl or F is used as the processing gas supplied into the processing chamber 102 by the gas supply unit 120. Specifically, in etching a silicon oxide film such as a SiO2 film, a fluorocarbon gas such as CxFy or CHF3 gas is used as the processing gas.

[0068] An exhaust unit 130 that exhausts the atmosphere inside the processing chamber 102 is connected to the bottom of the processing chamber 102 via an exhaust pipe 132. The exhaust unit 130 is configured, for example, by a vacuum pump, and is capable of reducing the pressure inside the processing chamber 102 to a predetermined level. A wafer loading / unloading port 134 is formed in a sidewall of the processing chamber 102, and a gate valve 136 is provided at the wafer loading / unloading port 134. For example, when loading a wafer W, the gate valve 136 is opened and the wafer W is placed on the mounting table 110 in the processing chamber 102 by a transfer mechanism such as a transfer arm (not shown), and the gate valve 136 is closed to process the wafer W.

[0069] A planar high-frequency antenna 140 and a shield member 160 covering the high-frequency antenna 140 are disposed on the upper surface (outer surface) of a plate-shaped dielectric 104 in the ceiling of the processing chamber 102. The high-frequency antenna 140 in this embodiment is roughly divided into an inner antenna element 142A disposed in the center of the plate-shaped dielectric 104 and an outer antenna element 142B disposed so as to surround the outer periphery of the inner antenna element 142A. Each of the antenna elements 142A, 142B is formed in a spiral coil shape made of a conductor such as copper, aluminum, or stainless steel.

[0070] The shield member 160 in this embodiment includes a cylindrical inner shield wall 162A provided between the antenna elements 142A and 142B so as to surround the inner antenna element 142A, and a cylindrical outer shield wall 162B provided so as to surround the outer antenna element 142B. This divides the upper surface of the plate-shaped dielectric 104 into a central portion (central zone) inside the inner shield wall 162A and a peripheral portion (peripheral zone) between the shield walls 162A and 162B.

[0071] A disk-shaped inner shield plate 164A is provided on the inner antenna element 142A so as to cover the opening of the inner shield wall 162A. A doughnut-shaped outer shield plate 164B is provided on the outer antenna element 142B so as to cover the opening between the shield walls 162A and 162B.

[0072] The shape of the shield member 160 is not limited to a cylindrical shape. The shape of the shield member 160 may be another shape, such as a rectangular tube, but it is preferable to match the shape of the processing chamber 102. Here, for example, the processing chamber 102 is approximately cylindrical, so the shield member 160 is also formed approximately cylindrical to match the shape of the processing chamber 102.

[0073] The antenna elements 142A and 142B are connected to radio frequency power sources 150A and 150B, respectively. This allows radio frequency waves of the same frequency or different frequencies to be applied to the antenna elements 142A and 142B. For example, when a radio frequency wave of a predetermined frequency (e.g., 40 MHz) is supplied to the inner antenna element 142A from the radio frequency power source 150A with a predetermined power, an induced magnetic field is formed in the processing chamber 102. The processing gas introduced into the processing chamber 102 is excited by the formed induced magnetic field, and a doughnut-shaped plasma is generated in the center above the wafer W.

[0074] Furthermore, when a high frequency power of a predetermined frequency (e.g., 60 MHz) is supplied to the outer antenna element 142B from the high frequency power supply 150B, an induced magnetic field is formed in the processing chamber 102. The processing gas introduced into the processing chamber 102 is excited by the formed induced magnetic field, and another doughnut-shaped plasma is generated on the peripheral portion of the wafer W.

[0075] These plasmas are used to perform predetermined plasma processing on the wafer, such as ashing, etching, and film formation. The high frequency output from each of the high frequency power supplies 150A and 150B is not limited to the above-mentioned frequencies. For example, high frequency waves of various frequencies such as 13.56 MHz, 27 MHz, 40 MHz, and 60 MHz can be supplied. However, it is necessary to adjust the electrical length of each of the antenna elements 142A and 142B according to the high frequency waves output from the high frequency power supplies 150A and 150B.

[0076] A control unit (overall control device) 200 is connected to the substrate processing apparatus 100, and each unit of the substrate processing apparatus 100 is controlled by the control unit 200. In addition, an operation unit 210 including a keyboard through which an operator inputs commands to manage the substrate processing apparatus 100, a display that visualizes and displays the operating status of the substrate processing apparatus 100, and the like is connected to the control unit 200.

[0077] Furthermore, the control unit 200 is connected to a storage unit 220 in which programs for implementing various processes executed in the substrate processing apparatus 100 under the control of the control unit 200, recipe data required to execute the programs, and the like are stored.

[0078] The storage unit 220 stores, for example, a plurality of process recipes for performing processes on the wafer W, as well as recipes for performing processes such as cleaning in the processing chamber 102. These recipes are a collection of a plurality of parameter values ​​such as control parameters and setting parameters for controlling each part of the substrate processing apparatus 100. For example, the process recipe has parameter values ​​such as the flow rate ratio of the processing gas, the pressure in the processing chamber 102, and the frequency and power of the high frequency waves applied to each of the antenna elements 142A and 142B.

[0079] These recipes may be stored in a hard disk or semiconductor memory, or may be stored on a portable computer-readable storage medium such as a CD-ROM or DVD and set in a predetermined position in the storage unit 220.

[0080] The control unit 200 reads out a desired process recipe from the storage unit 220 based on an instruction from the operation unit 210 and controls each unit to execute a desired process in the substrate processing apparatus 100. In addition, the recipe can be edited by operating the operation unit 210.

[0081] Although an ICP (Inductively Coupled Plasma) apparatus is shown as an example here, the substrate processing apparatus 100 may be a CCP (Capacitively Coupled Plasma) apparatus. In addition to the high-frequency antenna 140 provided on the ceiling of the processing chamber 102, high-frequency power may be supplied to a lower electrode constituting the mounting table 110 to generate plasma.

[0082] (Effects of the embodiment) The substrate processing method according to the embodiment includes a step of providing a substrate and a first step. In the step of providing a substrate, a substrate having a first film and a second film formed on the first film and having an opening formed therein is provided. In the first step, a first processing gas is turned into plasma to sputter the second film and etch the first film at the same time, while forming a protective film on the sidewall of the first film with a product generated by the sputtering. The substrate processing method according to the embodiment can proceed in parallel with the formation of the protective film by sputtering the second film and the etching of the first film. Therefore, according to the embodiment, the first film can be etched while suppressing bowing of the first film (organic film). Furthermore, according to the substrate processing method according to the embodiment, a protective film can be formed in a place where bowing is likely to occur, so that bowing can be effectively suppressed. The first step may be performed, for example, until the aspect ratio of the pattern formed on the first film is at least 5.

[0083] Moreover, the substrate processing method according to the above embodiment may further include a second step of etching the first film through the second film by converting the second processing gas into plasma.

[0084] In addition, the substrate processing method according to the above embodiment may further include a third step of forming a silicon-containing film on the top of the second film by plasmatizing the third processing gas. Therefore, according to the above embodiment, when the second film functioning as a mask is reduced, the third step is performed to stack the second film and continue etching. Therefore, according to the embodiment, a pattern with a high aspect ratio can be formed on the first film.

[0085] Moreover, the substrate processing method according to the above embodiment may further include a fourth step of converting a fourth processing gas into plasma to remove clogging material that blocks the opening and / or the upper part of the pattern generated in any of the first, second, and third steps. Therefore, according to the above embodiment, when there is a possibility that the opening or the upper part of the pattern may be clogged with a deposit, the fourth step is appropriately performed, whereby etching can be performed while suppressing clogging of the opening.

[0086] In addition, in the substrate processing method according to the above embodiment, a plurality of cycles each combining one or more arbitrary steps selected from the second step, the third step, and the fourth step may be performed in a predetermined order and number of times. Therefore, according to the above embodiment, the shape formed by etching can be controlled by performing a step suited to the progress of etching.

[0087] In the substrate processing method according to the above embodiment, a pattern having an aspect ratio of 20 or more may be formed in the first film.

[0088] In the substrate processing method according to the above embodiment, the first processing gas, which is a hydrogen-containing gas, may be turned into plasma to sputter the second film, which is an anti-reflection film.

[0089] Moreover, the substrate processing method according to the above embodiment may further include the step of etching the alternately laminated portion of the silicon oxide film and the silicon oxynitride film through the first film.

[0090] The substrate processing apparatus according to the embodiment includes a storage unit that stores a program for executing the substrate processing method, and a control unit that controls the execution of the program, so that the substrate processing apparatus according to the embodiment can control the pattern shape formed on the substrate by etching.

[0091] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. [Explanation of symbols]

[0092] 31 Insulating film 32 Organic film (film to be etched) 33 Silicon-containing films 40 Protective film 100 Substrate processing apparatus 102 Processing Room 110 Placement table S Laminated structure D product W wafer

Claims

1. A chamber; a stage for supporting a substrate within the chamber; A gas supply unit; A plasma generating unit; A control unit; Including, The control unit controls the gas supply unit and the plasma generation unit, a step of preparing a substrate on the mounting table, the substrate having a first film including an organic film and a second film on the first film, the second film having an opening; a third process of forming a film on the top of the second film by generating a third process gas into plasma; a fourth step of generating plasma from a fourth process gas to remove clogging material generated in the third step and clogging the opening and / or an upper portion of a pattern formed on the first film; a second process of etching the first film through the second film by generating plasma from a second processing gas; configured to perform a process including Substrate processing equipment.

2. The substrate processing apparatus according to claim 1 , wherein the control unit is configured to execute a process in which a cycle including the third process, the second process, and the fourth process is executed a plurality of times.

3. The substrate processing apparatus of claim 2 , wherein the control unit is configured to execute the cycle a plurality of times while changing processing conditions.

4. 4. The substrate processing apparatus of claim 1, wherein the control unit is configured to execute a process further including a first step of etching the first film while sputtering the second film by converting a first processing gas into plasma.

5. The substrate processing apparatus according to claim 4 , wherein the first step includes depositing a sputtering product produced by the sputtering on a side wall of the first film.

6. The substrate processing apparatus according to claim 4 , wherein the control unit is configured to execute a process of executing the first step after the preparing step and before the third step.

7. The step of preparing a substrate includes: providing a substrate including the first film, a second film on the first film, and a photoresist on the second film; etching the second film through the photoresist to form the opening in the second film; The substrate processing apparatus according to claim 1 , further comprising:

8. The substrate processing apparatus according to claim 7 , wherein the photoresist is an EUV resist.

9. The substrate processing apparatus according to claim 1 , wherein the first film includes an amorphous carbon film.

10. The substrate processing apparatus of claim 1 , wherein the second film includes a silicon-containing film.

11. 10. The substrate processing apparatus according to claim 1, wherein the second film includes a SiO2 film, a SiN film, a SiON film, a Poly-Si film, or a SiCN film.

12. The substrate processing apparatus according to claim 1 , wherein the second film includes an anti-reflective film.

13. The substrate processing apparatus according to claim 1 , wherein the plasma generating unit includes a high-frequency antenna disposed on a ceiling of the chamber.

14. A chamber; a stage for supporting a substrate within the chamber; A gas supply unit; A plasma generating unit; A control unit; Including, The control unit controls the gas supply unit and the plasma generation unit, preparing a substrate having a first film and a second film on the first film, the second film having an opening; a third process of forming a film on the top of the second film by generating a third process gas into plasma; a second process of etching the first film through the second film by generating plasma from a second processing gas; a fourth step of generating plasma from a fourth process gas to remove clogging material generated in the third step and clogging the opening and / or an upper portion of a pattern formed on the first film; The substrate processing apparatus is configured to perform a process including:

15. The substrate processing apparatus according to claim 14 , wherein the control unit is configured to execute a process in which a cycle including the third process, the second process, and the fourth process is executed a plurality of times.

16. The substrate processing apparatus of claim 15 , wherein the controller is configured to perform the cycle multiple times while changing processing conditions.

17. A step of preparing a substrate having a first film including an organic film and a second film on the first film on a mounting table in a chamber, the second film having an opening; a third process of forming a film on the top of the second film by generating a third process gas into plasma; a fourth step of generating plasma from a fourth process gas to remove clogging material generated in the third step and clogging the opening and / or an upper portion of a pattern formed on the first film; a second process of etching the first film through the second film by generating plasma from a second processing gas; A method for processing a substrate, comprising:

Citation Information

Patent Citations

  • Method for plasma etching performance enhancement

    JP2008060566A

  • Manufacturing method of semiconductor device, and storage medium

    JP2009049141A

  • Method for manufacturing semiconductor device

    JP2009076661A

  • Substrate treatment method

    JP2010153702A

  • Plasma etching method and plasma etching device

    JP2012138520A