Light reflective resin film
The light-reflecting resin film with controlled refractive index and melt resistance layers, along with protective layers, addresses adhesion issues, improving optical reliability and process stability by preventing defects and ensuring uniform adhesion.
Patent Information
- Application Number
- JP2023166058
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-04-06
- Filing Date
- 2023-09-27
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-04-05
AI Technical Summary
Existing light-reflecting resin films face issues with poor adhesion between layers, leading to optical defects such as uneven patterns and banding due to variations in refractive index and melt resistance, which affect optical reliability and process stability.
A light-reflecting resin film with alternating resin layers having specific refractive index differences, melt resistance, and glass transition temperature ranges, along with protective layers, is manufactured using controlled extrusion and stretching processes to ensure uniform adhesion and prevent defects.
The solution enhances optical reliability by preventing optical and mechanical defects, ensuring uniform adhesion and stability during the casting process, and maintaining desired light reflection characteristics.
Smart Images

Figure 0007566108000017 
Figure 0007566108000018 
Figure 0007566108000019
Abstract
Description
[Technical field]
[0001] The present invention relates to a light reflecting resin film and a method for producing the same, and more particularly to a light reflecting resin film including a plurality of resin layers and a method for producing the same. [Background technology]
[0002] Polymer films are widely used in the fields of electronics, chemistry, food, medicine, construction, packaging, etc. For example, in the case of decorative polymer films having a specific color, a colorant can be used, or a method of reflecting or blocking light of a specific wavelength can be used.
[0003] For example, by repeatedly laminating resin layers having different refractive indices, it is possible to produce a light reflective film that can selectively reflect light having a wavelength in a specific range, such as an infrared reflective film, a visible light reflective film, or a polarized light reflective film.
[0004] However, when multiple resin layers are laminated together, poor adhesion between the resin layers may occur, for example, the resin layers may be bonded together during co-extrusion, casting, etc., and optical defects such as uneven patterns, banding patterns, etc. may occur due to fluctuations in optical properties.
[0005] Therefore, it is necessary to develop a composition or process for a light reflective resin film that improves optical reliability while maintaining light reflection characteristics of a desired wavelength due to the refractive index difference.
[0006] For example, Korean Patent Publication No. 2003-0012874 discloses an infrared reflective film having a multi-layer structure. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Korean Patent Publication No. 2003-0012874 Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the exemplary embodiments is to provide a light-reflecting resin film having improved optical properties and process stability, and a manufacturing method thereof. [Means for solving the problem]
[0009] The light-reflecting resin film according to an exemplary embodiment includes a reflective stack including a resin layer, and the melt resistance of the resin layer is 2,000 MΩ or less, which is measured by contacting a copper plate with the resin layer in a molten film form and applying a voltage of 50 V to the copper plate.
[0010] In some embodiments, the reflective stack may include a first resin layer and a second resin layer alternately stacked, and the refractive index of the first resin layer may be greater than the refractive index of the second resin layer.
[0011] In some embodiments, the melt resistance of each of the first resin layer and the second resin layer may be 2,000 MΩ or less.
[0012] In some embodiments, the first resin layer and the second resin layer may each have a melt resistance of 50 to 500 MΩ.
[0013] In some embodiments, the first resin layer and the second resin layer can satisfy an F-ratio defined by the following formula 1 in the range of 0.35 to 0.65.
[0014]
number
[0015] (In formula 1, n 1 and n 2 are the refractive indices of the first resin layer and the second resin layer, respectively, and d 1 and d 2are the thicknesses of the first and second resin layers, respectively.)
[0016] In some embodiments, the first resin layer may include polyethylene terephthalate (PET) and the second resin layer may include polymethyl methacrylate (PMMA). The melt resistance of the first resin layer may be measured at 280°C and the melt resistance of the second resin layer may be measured at 240°C.
[0017] In some embodiments, each of the first resin layer and the second resin layer may include a resistance modifier including an alkali metal salt or an alkaline earth metal salt.
[0018] In some embodiments, the light-reflecting resin film may further include a first protective layer and a second protective layer laminated on the top and bottom surfaces of the reflective stack, respectively.
[0019] A light-reflecting resin film according to an exemplary embodiment includes a reflective stack in which a first resin layer containing a first polymer and a second resin layer containing a second polymer are alternately laminated, the second resin layer having a smaller refractive index than the first resin layer, and the second polymer satisfies the following formula 3.
[0020]
number
[0021] (In formula 3, α is in the range of −8,800 to −8,100, β is 260,000, and the MFI value is the value obtained by removing the unit expressed in g / min from the measured MFI.)
[0022] In some embodiments, the glass transition temperature (Tg) difference between the second polymer and the first polymer may be 15° C. or less.
[0023] In some embodiments, the second polymer may have a glass transition temperature greater than the glass transition temperature of the first polymer, and the glass transition temperature of the second polymer may be between 80 and 100°C.
[0024] In some embodiments, the second polymer may have a weight average molecular weight (Mw) of 100,000 or more.
[0025] In some embodiments, the weight average molecular weight (Mw) of the first polymer may range from 30,000 to 100,000.
[0026] In some embodiments, the first polymer can include polyethylene terephthalate (PET) and the second polymer can include polymethyl methacrylate (PMMA).
[0027] In some embodiments, the first resin layer and the second resin layer can satisfy an F-ratio defined by the following formula 1 in the range of 0.35 to 0.65.
[0028]
number
[0029] (In formula 1, n 1 and n 2 are the refractive indices of the first resin layer and the second resin layer, respectively, and d 1 and d 2 are the thicknesses of the first and second resin layers, respectively.)
[0030] In some embodiments, the weight ratio of the first polymer to the second polymer may be from 1.7 to 3.
[0031] Some embodiments may further include first and second protective layers deposited on the top and bottom surfaces of the reflective stack, respectively.
[0032] In some embodiments, the reflective stack may have a longitudinal stretch ratio of 3.3 or more.
[0033] In a method for producing a light-reflecting resin film according to an exemplary embodiment, a first resin raw material containing a first polymer and a first resistance adjuster and a second resin raw material containing a second polymer and a second resistance adjuster are prepared. The first resin raw material and the second resin raw material are extruded to form a pre-melted laminate including a first molten film and a second molten film that are alternately and repeatedly arranged. A voltage is applied to bring the pre-melted laminate into close contact with a casting roll to form a pre-reflective stack. The pre-reflective stack is stretched.
[0034] In some embodiments, the melt resistance of each of the first molten film and the second molten film is 2,000 MΩ or less, and the melt resistance can be measured by adjacent a copper plate to each of the first molten film and the second molten film and applying a voltage of 50 V to the copper plate. Effect of the Invention
[0035] According to the above-mentioned exemplary embodiment, the resin layer included in the light-reflecting resin film has a melt resistance value within a predetermined range, which allows the resin layer to have appropriate electrical conductivity, thereby ensuring uniform adhesion characteristics in a casting process for forming a resin laminate, and preventing the occurrence of optical defects such as band patterns and uneven patterns.
[0036] According to an exemplary embodiment, the resin layer may include a base polymer and a resistance adjuster mixed with the base polymer. The melt resistance can be controlled by adjusting the content of the resistance adjuster, and the color change of the resin layer such as yellowing can be suppressed while preventing the above-mentioned optical defects.
[0037] According to another exemplary embodiment, the light reflecting resin film may include a first resin layer including a first polymer and a second resin layer including a second polymer. The weight average molecular weight and melt flow index of the second polymer may be adjusted to satisfy a predetermined relationship in consideration of compatibility with the first resin layer.
[0038] This improves the stability of the stretching process of the light reflective resin film, the stability of the product formation, and improves the interlayer consistency, thereby suppressing or reducing optical and mechanical defects such as scratches and banding patterns.
[0039] In some embodiments, the difference in glass transition temperature between the first polymer and the second polymer is maintained within a predetermined range, and film formation stability and stretching stability can be further improved. [Brief description of the drawings]
[0040] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a light reflecting resin film according to an exemplary embodiment. [Diagram 2] FIG. 2 is a schematic diagram showing a method for producing a light reflecting resin film according to an exemplary embodiment. [Diagram 3] FIG. 3 is a schematic diagram showing a method for producing a light reflecting resin film according to an exemplary embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0041] According to an exemplary embodiment, a light reflecting resin film having improved optical reliability and a method for manufacturing the same are provided.
[0042] Hereinafter, the embodiments of the present invention will be described in detail. However, since the present invention can be modified in various ways and can have various forms, a specific embodiment will be illustrated in the drawings and described in detail in the present text. However, this is not intended to limit the present invention to the specific disclosed form, and it should be understood that the present invention includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention.
[0043] Unless otherwise defined, all terms used herein, including technical or scientific terms, have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. Terms as defined in commonly used dictionaries should be interpreted as having a meaning consistent with the meaning they have in the context of the relevant art, and should not be interpreted in an idealized or overly formal sense unless expressly defined in this application.
[0044] FIG. 1 is a schematic cross-sectional view showing a light reflecting resin film according to an exemplary embodiment.
[0045] 1, the light reflecting resin film 100 may include a reflecting stack 110 and protective layers 150a, 150b. According to an exemplary embodiment, the reflecting stack 110 may include a first resin layer 120 and a second resin layer 130.
[0046] The first resin layer 120 and the second resin layer 130 may have different refractive indices. Due to the difference in refractive index between the first resin layer 120 and the second resin layer 130, the reflective stack 110 may achieve light reflection or light blocking performance due to interface reflection.
[0047] In one embodiment, the refractive index difference between the first resin layer 120 and the second resin layer 130 may be 0.01 or more, preferably 0.05 or more, and more preferably 0.1 or more.
[0048] The first resin layer 120 and the second resin layer 130 may contain an appropriate polymer within a range that maintains the refractive index difference described above.
[0049] The first resin layer 120 may include a first polymer having a higher refractive index than the second resin layer 130. For example, it may include a polyester-based polymer, a polyester-based copolymer, polynaphthalene, etc. In one embodiment, the first resin layer 120 includes polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PEN), etc. In a preferred embodiment, the first resin layer 120 or the first polymer may include polyethylene terephthalate (PET). For example, the first resin layer 120 may have a higher refractive index than the second resin layer 130.
[0050] For example, the refractive index of the first resin layer 120 is in the range of 1.6 to 1.7, and when the first resin layer 120 contains PET, it can have a refractive index in the range of 1.64 to 1.66.
[0051] The first resin layer 120 may have birefringence properties. As described above, the first resin layer 120 may contain PET, and may have positive birefringence properties in which the refractive index increases by stretching.
[0052] The melting temperature of the first resin layer 120 may be, for example, 270° C. or higher. In one embodiment, the melting temperature of the first resin layer 120 may be in the range of 270 to 290° C.
[0053] In some embodiments, the glass transition temperature of the first polymer may be in the range of 75 to 85° C. for ease of melting and extrusion processes.
[0054] In some embodiments, the weight average molecular weight (Mw) of the first polymer may be in the range of about 30,000 to 100,000. Within this range, film formation stability and stretching stability can be improved. In a preferred embodiment, the weight average molecular weight of the first polymer may be in the range of about 40,000 to 80,000.
[0055] The second resin layer 130 may include a second polymer having a lower refractive index than the first polymer of the first resin layer 120. For example, it may include an acrylic polymer such as polymethyl methacrylate (PMMA), polystyrene (PS), polyvinyl fluoride (PVF), polyvinylidene fluoride (PVDF), polylactic acid (PLA), etc. In a preferred embodiment, the second resin layer 130 may include PMMA. For example, the second resin layer 130 may have a lower refractive index than the first resin layer 120.
[0056] In some embodiments, the second resin layer 130 may include a copolymerized polyester polymer. For example, the second resin layer may include a copolymer (co-PET) in which polyethylene terephthalate (PET) is copolymerized with neopentyne glycol (NPG), cyclohexanedimethanol (CHDM), and / or syndiotactic polystyrene (SPS).
[0057] For example, the refractive index of the second resin layer 130 is in the range of 1.4 to 1.5, and when the second resin layer 130 contains PMMA, it can have a refractive index in the range of 1.485 to 1.495.
[0058] The second resin layer 130 may include an isotropic polymer. As described above, the second resin layer 130 may include PMMA, the refractive index of which does not change due to stretching. In this case, the refractive index of the first resin layer 120 may increase due to stretching, and the refractive index difference between the first resin layer 120 and the second resin layer 130 may increase.
[0059] The melting temperature of the second resin layer 130 may be, for example, 210° C. or higher. In one embodiment, the melting temperature of the second resin layer 130 may be in the range of 210 to 240° C.
[0060] According to an exemplary embodiment, the glass transition temperature (Tg) of the second polymer contained in the second resin layer 130 can be adjusted taking into consideration, for example, the ease of co-extrusion with the first polymer including PET and flow stability.
[0061] In some embodiments, the difference in glass transition temperature (Tg) between the second polymer and the first polymer may be 15° C. or less. In one embodiment, the glass transition temperature (Tg) of the second polymer may be 80 to 100° C. while maintaining the glass transition temperature difference range.
[0062] 1, the reflective stack 110 may include a first resin layer 120 and a second resin layer 130 that are alternately and repeatedly stacked. For example, the number of layers in the reflective stack 110 may be in the range of 100 to 200. In a preferred embodiment, the number of layers in the reflective stack 110 may be in the range of 140 to 160.
[0063] In some embodiments, the F-ratio of the reflective stack 110, as defined by the following Equation 1, can be adjusted in the range of 0.35 to 0.65.
[0064]
number
[0065] (In formula 1, n 1 and n 2 are the refractive indices of the first resin layer 120 and the second resin layer 130, respectively, and d 1 and d 2 are the thicknesses of the first resin layer 120 and the second resin layer 130, respectively.)
[0066] The light irradiated to the light reflecting resin film 100 forms a primary reflection wavelength at the wavelength (λ) and can form a secondary reflection wavelength at, for example, λ / 2 wavelength. If the reflectance at the secondary reflection wavelength is high, the light reflection may increase too much at wavelengths in an undesired band.
[0067] By adjusting the F ratio within the above-mentioned range, excessive light reflection at the reflection wavelength can be suppressed, and the second reflection wavelength can be selectively utilized together with the first reflection wavelength.
[0068] In one embodiment, the F ratio can be adjusted to a range of 0.45 to 0.55, in which case the second reflected wavelength is substantially eliminated and only the first reflected wavelength can be utilized.
[0069] The refractive index and thickness of each of the first resin layer 120 and the second resin layer 130 can be appropriately designed according to the desired wavelength of reflected light while maintaining the above-mentioned F ratio.
[0070] For example, the refractive index and thickness of each of the first resin layer 120 and the second resin layer 130 can be determined according to the desired wavelength (λ) of blocked light using the following formula 2.
[0071]
number
[0072] In formula 2, n 1 and n 2 are the refractive indices of the first resin layer 120 and the second resin layer 130, respectively, and d 1 and d 2 are the thicknesses of the first resin layer 120 and the second resin layer 130, respectively.
[0073] According to an exemplary embodiment, the reflective stack 110 may have a melt resistance of 500 MΩ or less. According to an exemplary embodiment, the first resin layer 120 and the second resin layer 130 may each have a melt resistance of 2,000 MΩ or less.
[0074] If the melt resistance of the first resin layer 120 and the second resin layer 130 exceeds 2,000 MΩ, the electrical conductivity may not be fully realized in the casting process, as described later in Fig. 2. This may result in poor adhesion to the casting roll, causing band patterns or uneven patterns in the TD or lateral directions.
[0075] In a preferred embodiment, the melt resistance of the first resin layer 120 and the second resin layer 130 may be in the range of 50 to 500 MΩ. In this range, the reliability of the casting process is improved by uniform current flow, and discoloration of the resin layer, such as yellowing, caused by an increase in the content of a resistance adjuster described below can be prevented.
[0076] The melt resistance is a resistance value measured by applying a voltage of 50 V to each of the first resin layer 120 and the second resin layer 130, which are in the form of a film in a molten state, while being spaced a predetermined distance from a copper (Cu) plate. For example, the size of the copper plate may be 25 mm wide x 200 mm long x 2 mm thick. The distance between the copper plate and the resin layer may be 30 mm.
[0077] When the first resin layer 120 includes PET, the melt resistance of the first resin layer 120 can be measured at 280° C. When the second resin layer 130 includes PMMA, the melt resistance of the second resin layer 130 can be measured at 240° C.
[0078] According to an exemplary embodiment, the first resin layer 120 and the second resin layer 130 may each include a resistance adjuster. In some embodiments, the melt resistance in the aforementioned range can be achieved by adjusting the content of the resistance adjuster.
[0079] The resistance regulator may include an alkali metal salt or an alkaline earth metal salt. For example, the resistance regulator may include an inorganic salt such as potassium halide, magnesium halide, potassium hydroxide, magnesium hydroxide, or an organic salt such as potassium acetate, magnesium acetate, or the like. These may be used alone or in combination of two or more.
[0080] According to some embodiments, the content of the resistance adjuster in the first resin layer 120 may be 10 ppm or more based on the total weight of the first polymer, such as PET, contained in the first resin layer 120. In a preferred embodiment, the content of the resistance adjuster in the first resin layer 120 may be in the range of 50 to 300 ppm, more preferably 50 to 200 ppm, based on the total weight of the first polymer.
[0081] According to some embodiments, the content of the resistance adjuster in the second resin layer 130 may be 100 ppm or more based on the total weight of the second polymer, such as PMMA, contained in the second resin layer 130. In a preferred embodiment, the content of the resistance adjuster in the second resin layer 130 may be in the range of 100 to 300 ppm, more preferably 100 to 200 ppm, based on the total weight of the second polymer.
[0082] According to another exemplary embodiment, the weight average molecular weight (Mw) and melt flow index (MFI) of the second polymer contained in the second resin layer 130 can be determined taking into consideration the lamination compatibility with the first resin layer 120 and the stretching stability.
[0083] For example, if the lamination consistency between the first resin layer 120 and the second resin layer 130 decreases, interfacial peeling may occur within the reflective stack 110, and breakage, cracks, etc. may occur due to differences in physical properties between the layers during the stretching process.
[0084] Furthermore, band patterns may occur due to flow inconsistency at the interface between the first resin layer 120 and the second resin layer 130 during the extrusion process, and scratches, stains, and the like may occur during the rolling process.
[0085] According to an exemplary embodiment, the second polymer can satisfy Formula 3 below:
[0086]
number
[0087] (In formula 3, α is in the range of −8,800 to −8,100, and β is 260,000. The MFI value in formula 3 means the value obtained by removing the unit from the measured MFI.)
[0088] The melt flow index (MFI) included in Equation 3 is measured under conditions of 230°C and 3.80 kg, and is expressed in units of g / min.
[0089] For example, the second polymer can have a weight average molecular weight (Mw) and a melt flow index (MFI) value that have a substantially linear relationship within the range of α provided by the slope in Equation 3.
[0090] When the relationship defined by the above formula 3 is satisfied, optical defects, mechanical defects, etc. caused by the insufficient interlayer matching described above can be effectively suppressed or significantly reduced.
[0091] In some embodiments, the weight average molecular weight of the second polymer may be greater than or equal to about 100,000, and preferably in the range of about 100,000 to 200,000.
[0092] 1, a first protective layer 150a and a second protective layer 150b may be laminated, respectively, on the top and bottom surfaces of the reflective stack 110. For example, the first protective layer 150a and the second protective layer 150b may include a PET film.
[0093] In some embodiments, the thickness of the reflective stack 110 may be about 50-70%, preferably about 50-60%, of the total thickness of the light reflecting resin film 100. Within this range, the film protection by the protective layers 150a and 150b and the light transmittance of the light reflecting resin film 100 are not excessively hindered, and the reflection / blocking of a desired wavelength band can be effectively achieved.
[0094] 2 and 3 are schematic diagrams showing a method for producing a light reflecting resin film according to an exemplary embodiment.
[0095] 2, the resin raw material 50 can be melted and extruded by an extruder 60. The resin raw material 50 can separately contain a first resin raw material containing the above-mentioned first polymer and a second resin raw material containing the above-mentioned second polymer.
[0096] In an exemplary embodiment, the first resin feedstock and the second resin feedstock may each further include a resistance modifier.
[0097] The first resin raw material and the second resin raw material may be manufactured in the form of pellets or chips, respectively, and fed into the extruder 60. According to an exemplary embodiment, the weight ratio or extrusion rate ratio of the first resin raw material to the second resin raw material may be 1.7 to 3. Within this range, it is possible to prevent wavy patterns and deformation of the film caused by interfacial flow resulting from the viscosity difference between the first polymer and the second polymer.
[0098] In a preferred embodiment, the weight ratio or extrusion rate ratio may be in the range of 2 to 2.7.
[0099] The resin raw material 50 can be melted and extruded by the extruder 60 and moved through a conveying line 70. The resin raw material 50 can then be discharged through an extrusion die 80 in the form of a molten film.
[0100] 3, the first resin raw material and the second resin raw material can be moved and supplied via a first transfer line 72 and a second transfer line 74, respectively. Then, a first molten film produced from the first resin raw material and a second molten film produced from the second resin raw material can be discharged from a first extrusion die 82 and a second extrusion die 84 connected to the first transfer line 72 and the second transfer line 74, respectively.
[0101] The first extrusion die 82 and the second extrusion die 84 can be arranged alternately and repeatedly, whereby the first molten film and the second molten film can be discharged alternately and repeatedly to obtain a pre-molten laminate.
[0102] Returning to FIG. 2, the pre-molten laminate exiting the extrusion die 80 may be fed to a casting roll 90 .
[0103] According to an exemplary embodiment, an electrostatic applicator 85 can be disposed adjacent to the casting roll 90. For example, the electrostatic applicator 85 can be disposed to face the casting roll 90 across the pre-molten laminate. The electrostatic applicator 85 can include a metal conductor or a metal plate, such as a copper conductor or a copper plate, connected to a power source.
[0104] When a voltage is applied to the electrostatic application section 85 via the power supply, a negative charge is induced in the cast roller 90, and the resistance adjuster contained in the first molten film and the second molten film enables the pre-molten laminate to adhere to the cast roller 90.
[0105] As described above, each of the first molten film and the second molten film can have a melt resistance of 2,000 MΩ or less, preferably in the range of 50 to 500 MΩ, which can increase adhesion to the cast roller 90 by electrical attraction when applying electricity or static electricity, and can prevent optical defects due to insufficient electricity.
[0106] In some embodiments, the temperature of the casting roller 90 can be maintained at or below room temperature, so that the pre-molten laminate can be solidified in close contact with the casting roller 90 by energizing as described above to form a preliminary reflective stack.
[0107] The pre-reflective stack may be tensioned and moved by a tensioner 95 .
[0108] Thereafter, the preliminary reflective stack can be stretched by a stretching roller or the like to obtain the reflective stack 110. As shown in Fig. 1, a first protective layer 150a and a second protective layer 150b can be laminated on the top and bottom surfaces of the reflective stack 110, respectively, to manufacture the light reflective resin film 100. In one embodiment, a stretching process can be performed after the first protective layer 150a and the second protective layer 150b are laminated.
[0109] The stretching step may include stretching in the MD direction (e.g., stretching in the longitudinal direction) and stretching in the TD direction (e.g., stretching in the transverse direction). For example, the stretch ratio in the longitudinal direction may be 3.3 times or more. In this case, the film is prevented from breaking or breaking in the transverse direction stretching after the longitudinal stretching, and a stable tensile strength can be maintained.
[0110] According to the exemplary embodiment described above, the first resin raw material includes, for example, PET, and the second resin raw material can be obtained from a second polymer whose weight average molecular weight and melt flow index are adjusted as described above, and whose glass transition temperature difference with the first resin raw material is adjusted to be equal to or lower than a predetermined temperature.
[0111] This makes it possible to suppress the occurrence of undesired patterns due to uneven flow during the formation of the pre-molten laminate. Also, the adhesion stability on the casting roll 90 is improved, and scratches, roll marks, etc. caused by the casting roll 90, tensioner 95, etc. can be prevented.
[0112] In addition, the lamination stability of the reflective stack 110 is improved, and the stretching process can be performed stably, thereby allowing the stretch ratio to be further increased.
[0113] In the following, preferred examples are presented to aid in understanding the present invention, but these examples are merely illustrative of the present invention and do not limit the scope of the appended claims. It is clear to those skilled in the art that various changes and modifications can be made to these examples within the scope of the scope and technical ideas of the present invention, and it is natural that these changes and modifications fall within the scope of the appended claims.
[0114] Experimental Example 1 (1) Examples 1 to 8 and Comparative Examples 1 to 4 A pellet-shaped first resin raw material (containing a first polymer and a first resistance adjuster) and a second resin raw material (containing a second polymer and a second resistance adjuster) having the composition and contents shown in Table 1 were each melted and extruded by an extruder, and the first molten film and the second molten film were repeatedly supplied alternately through a feed block die including an extrusion die to form a pre-molten laminate of a total of 143 layers.
[0115] The melting and extrusion temperature of the first resin material was maintained at 280° C., and the melting and extrusion temperature of the second resin material was maintained at 240° C. The weight ratio of the first resin material to the second resin material was maintained at 2:1.
[0116] Thereafter, as described with reference to FIG. 2, the pre-molten laminate was supplied between a casting roller adjusted to 20° C. and a copper conductor, and a voltage was applied to the copper conductor to carry out a casting process.
[0117] Next, the pre-melted laminate that had been adhered and solidified by the casting roller was pulled by a tension roller to form a reflective stack including a first resin layer and a second resin layer that were alternately and repeatedly laminated. The first resin layer was formed to a thickness of 140 nm, and the second resin layer was formed to a thickness of 155 nm.
[0118] PET resin was applied to the top and bottom surfaces of the reflective stack to form a protective layer, and the stack was stretched 3.5 times in the vertical direction and 4.5 times in the horizontal direction to produce a light-reflective resin film.
[0119] [Table 1]
[0120] [Table 2]
[0121] [Table 3]
[0122] (2) Evaluation example 1) Melting resistance measurement The first and second molten films formed from the first and second resin raw materials, respectively, were placed on a copper plate, and a voltage of 50 V was applied to the copper plate. Thereafter, the resistance values in the first and second molten films were measured. As described above, the resistance measurement temperature of the first molten film was 280°C, and the resistance measurement temperature of the second molten film was 240°C.
[0123] 2) Evaluation of the occurrence of patterns in the TD direction The light reflecting resin films produced in the examples and comparative examples were observed visually and with a polarizing device (model number: LSM-401, manufactured by LUCEO Corporation) to evaluate the presence or absence of unevenness in the TD direction.
[0124] The evaluation criteria are as follows: ◯: No pattern is visible to the naked eye or with a polarizing device. △: The pattern is not visible to the naked eye, but is visible using a polarizing device. ×: The pattern is visible both to the naked eye and with a polarizing device.
[0125] The evaluation results are shown in Tables 4 and 5 below.
[0126] [Table 4]
[0127] [Table 5]
[0128] Referring to Tables 4 and 5, in the comparative examples in which the melt resistance of the first resin layer or the second resin layer exceeded 2,000 MΩ, patterns in the TD direction were visually observed.
[0129] In contrast, in the cases of Examples 1 to 5 in which both the first and second resin layers had a melt resistance of 500 MΩ or less, no pattern in the TD direction was observed visually or with a polarizing device.
[0130] However, in the case of Example 5 in which the melt resistance of the second resin layer was too reduced, discoloration of the second resin layer was observed due to an excessive increase in the content of the resistance adjuster.
[0131] Experimental Example 2 (1) Examples 9 to 14 and Comparative Examples 5 to 6 1) Example 9 i) Preparation of the first polymer (PET) A slurry prepared by mixing 358 parts by mass of high-purity terephthalic acid and 190 parts by mass of ethylene glycol per unit time was continuously fed into a reactor maintained under conditions of 274.5°C and normal pressure under a nitrogen atmosphere. The esterification reaction was completed within a theoretical residence time of 4 hours in the reactor while distilling off water and ethylene glycol generated in the esterification reaction outside the reactor.
[0132] 450 parts by mass of ethylene terephthalate oligomer formed in the esterification reaction was transferred to a polycondensation reaction tank. The reaction temperature in the polycondensation reaction tank was maintained at 276.5°C, the reaction pressure was maintained at 60 Pa, and the polycondensation reaction was carried out in a molten state for a residence time of 180 minutes while removing water and ethylene glycol generated in the polycondensation reaction from the polycondensation reaction tank, to obtain a polyethylene terephthalate (PET) resin.
[0133] ii) Preparation of the second polymer (PMMA) Based on 100 parts by weight of the monomer mixture, 96 parts by weight of methyl methacrylate, 4 parts by weight of methyl acrylate, 0.1 parts by weight of 2,2'-azobis(2,4-dimethyl-valeronitrile) as an initiator, and 1,1,3,3-tetramethylbutyl peroxy 2-ethyl hexanoate were used. The mixture was polymerized for 120 minutes at an initial reaction temperature of 60° C. using 0.03 parts by weight of methyl methacrylate-methacrylic acid copolymer, 133 parts by weight of water, 0.82 parts by weight of an aqueous solution of methyl methacrylate-methacrylic acid copolymer saponified with NaOH as a suspending agent, 0.098 parts by weight of sodium dihydrogen phosphate and 0.053 parts by weight of disodium hydrogen phosphate as buffer salts, and 0.33 parts by weight of normal-octyl mercaptan as a chain transfer agent.
[0134] Thereafter, the temperature was raised to 105° C. for 50 minutes, and polymerization was continued for a further 40 minutes to obtain polymethyl methacrylate (PMMA).
[0135] iii) Manufacturing of light-reflecting resin film A first resin raw material containing the first polymer in pellet form and a second resin raw material containing the second polymer were each melted and extruded by an extruder, and the first molten film and the second molten film were repeatedly supplied alternately by a feed block die including an extrusion die to form a pre-molten laminate having a total of 143 layers.
[0136] The melting and extrusion temperature of the first resin material was maintained at 280° C., and the melting and extrusion temperature of the second resin material was maintained at 240° C. The weight ratio of the first resin material to the second resin material was maintained at 2:1.
[0137] Thereafter, as described with reference to FIG. 2, the pre-molten laminate was supplied between a casting roller adjusted to 20° C. and a copper conductor, and a voltage was applied to the copper conductor to carry out a casting process.
[0138] Next, the pre-melted laminate that had been adhered and solidified by the casting roller was pulled by a tension roller to form a reflective stack including a first resin layer and a second resin layer that were alternately and repeatedly laminated. The first resin layer was formed to a thickness of 140 nm, and the second resin layer was formed to a thickness of 155 nm.
[0139] 2) Example 10 A light reflective resin film was produced in the same manner as in Example 9, except that the content of the chain transfer agent in the production process of the second polymer (PMMA) was adjusted to 0.25 parts by weight.
[0140] 3) Example 11 A light reflecting resin film was produced in the same manner as in Example 9, except that the additional polymerization time in the production process of the second polymer (PMMA) was adjusted to 30 minutes.
[0141] 4) Example 12 A light reflective resin film was produced in the same manner as in Example 9, except that the additional polymerization time in the production process of the second polymer (PMMA) was adjusted to 30 minutes and the additional polymerization temperature was adjusted to 95°C.
[0142] 5) Example 13 A light reflective resin film was produced in the same manner as in Example 12, except that the polycondensation time in the production process of the first polymer (PET) was increased to 300 minutes.
[0143] 6) Example 14 A light reflective resin film was produced in the same manner as in Example 12, except that the polycondensation time in the production step of the first polymer (PET) was reduced to 150 minutes.
[0144] 7) Comparative Example 5 A light reflective resin film was produced in the same manner as in Example 9, except that the content of the chain transfer agent in the production process of the second polymer (PMMA) was adjusted to 0.25 parts by weight and the additional polymerization time was adjusted to 30 minutes.
[0145] 8) Comparative Example 6 A light reflective resin film was produced in the same manner as in Example 9, except that the additional polymerization time in the production process of the second polymer (PMMA) was adjusted to 20 minutes.
[0146] The physical properties of the first polymer (PET) and the second polymer (PMMA) in the examples and comparative examples are shown in Tables 6 and 7 below.
[0147] Specifically, the glass transition temperature was measured using a DSC Q-2000 manufactured by TA Instruments, the weight average molecular weight (Mw) was measured using gel permeation chromatography (GPC) (PL-GPC220 manufactured by Agilent) and polystyrene standards, and the melt flow index (MFI) was measured in accordance with ASTM D1238 (measurement temperature: 230°C, load: 3.80 kg).
[0148] The α value of each of the second polymers was calculated from the above formula 3.
[0149] [Table 6]
[0150] [Table 7]
[0151] (2) Evaluation example 1) Evaluation of breakability The reflective stacks manufactured according to the above examples and comparative examples were coated with PET resin to form protective layers on the top and bottom surfaces, and then stretched 3.5 times in the vertical direction and 5.5 times in the horizontal direction to manufacture light-reflective resin films. The occurrence of breakage during the biaxial stretching process was observed and evaluated as follows.
[0152] <Evaluation criteria for breakability> ○: No breakage occurs. ×: Fracture occurs in at least one layer.
[0153] 2) Measurement of film tensile strength The tensile strength of the reflective stacks produced by the above Examples and Comparative Examples was measured using a JIS B 7721 tensile tester.
[0154] 3) Evaluation of MD stretching performance The reflective stacks produced by the above Examples and Comparative Examples were stretched in the MD direction, and the ratio of the MD length stretched to the breaking point to the initial MD length was measured.
[0155] <Evaluation Criteria for MD Stretching Performance> ○: Stretching exceeding 3.3 times the initial length is possible. △: Stretching between 3.1 times and 3.3 times the initial length is possible. ×: Stretching less than 3.1 times the initial length is possible.
[0156] 4) Evaluation of post-processing properties The reflective stacks produced by the above Examples and Comparative Examples were woven (post-processed) into yarns with a diameter of 0.254 mm or more using a micro-slitting device, and the processability was evaluated according to the following criteria.
[0157] <Evaluation Criteria for Post-Processing Performance> ○: No breakage or fracture of the yarn / film is observed during weaving. ×: Breakage or fracture of the yarn / film is observed during weaving.
[0158] 5) Pattern development The reflective stacks produced by the above Examples and Comparative Examples were visually observed to determine whether band patterns or wave patterns were observed (no pattern observed: ○, pattern observed: ×). The evaluation results are shown in Table 8 below.
[0159]
Table 8
[0160] Referring to Tables 6 to 8, compared to Comparative Examples 5 and 6, in which ΔTg exceeds 15° C. and Mw of PMMA is less than 100,000, falling outside the range of α defined in Equation 1, the reflective stacks or light-reflective resin films produced in Examples 9 to 14 showed improved breakability, high film tensile strength, excellent MD stretching performance and post-processability.
[0161] In the case of the comparative example, the interfacial flowability between the first resin layer and the second resin layer decreased, and a band pattern or a wave pattern was visually observed. [Explanation of symbols]
[0162] 50:Resin raw material 60: Extruder 70:Conveyor line 80: Extrusion die 85: Electrostatic application section 90: Cast roll 100: Light-reflecting resin film 110: Reflection Stack 120: 1st resin layer 130: Second resin layer 150a: 1st protective layer 150b: 2nd protective layer
Claims
1. a reflective stack in which a first resin layer containing a first polymer and a second resin layer containing a second polymer are alternately and repeatedly laminated; The second resin layer has a refractive index smaller than that of the first resin layer, and the second polymer satisfies the following formula 3: the difference in glass transition temperature (Tg) between the second polymer and the first polymer is 15° C. or less; The weight average molecular weight (Mw) of the second polymer is 100,000 or more; the first polymer is polyethylene terephthalate (PET) and the second polymer is polymethyl methacrylate (PMMA); A light-reflecting resin film, wherein the weight ratio of the first polymer to the second polymer is 1.7 to 3. [0010] (In formula 3, α is in the range of −8,800 to −8,100, β is 260,000, and the MFI value is the value obtained by removing the unit expressed in g / min from the measured MFI, Mw is measured using gel permeation chromatography (GPC) and polystyrene standards, and MFI is measured at 230°C and 3.80 kg load according to ASTM D1238.
2. the second polymer has a glass transition temperature greater than the glass transition temperature of the first polymer; 2. The light reflecting resin film according to claim 1, wherein the second polymer has a glass transition temperature of 80 to 100°C.
3. 2. The light reflecting resin film according to claim 1, wherein the weight average molecular weight (Mw) of the first polymer is in the range of 30,000 to 100,000.
4. The light-reflecting resin film according to claim 1, wherein the first resin layer and the second resin layer satisfy an F-ratio defined by the following formula 1 in the range of 0.35 to 0.
65. [0025] (In formula 1, n 1 and n 2 are the refractive indices of the first resin layer and the second resin layer, respectively, and d 1 and d 2 are the thicknesses of the first resin layer and the second resin layer, respectively.)
5. The light reflective resin film of claim 1 , further comprising a first protective layer and a second protective layer laminated on the top and bottom surfaces of the reflective stack, respectively.
6. 2. The light reflective resin film of claim 1, wherein the longitudinal stretch ratio of the reflective stack is 3.3 times or more.
Citation Information
Patent Citations
Plastic laminate, preparation method thereof and plastic molded product
CN111844992A
Image display screen and image display unit
JP2003075920A
Film, its manufacturing process and capacitor made of it
JP2005289065A
Laminated film and its manufacturing method
JP2009012187A
Light-selective reflective film and light-selective reflective film for displays
JP2014081526A