Method for producing sulfide-based inorganic solid electrolyte material
By employing grinding balls with varying diameters, the production time for sulfide-based inorganic solid electrolyte materials is shortened, enhancing industrial viability and conductivity.
Patent Information
- Application Number
- JP2020074287
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-04-17
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-04-17
AI Technical Summary
Sulfide-based inorganic solid electrolyte materials are produced through a mechanical milling method that is time-consuming and not suitable for industrial production due to the lengthy vitrification process.
The vitrification process is accelerated by using a combination of grinding balls with different diameters in a specific ratio during mechanical processing.
This method significantly reduces the production time of sulfide-based inorganic solid electrolyte materials while maintaining high purity and improving lithium ion conductivity.
Smart Images

Figure 0007566484000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a sulfide-based inorganic solid electrolyte material. [Background technology]
[0002] Lithium-ion batteries are generally used as power sources for small portable devices such as mobile phones and laptops, etc. Recently, lithium-ion batteries have also begun to be used as power sources for electric vehicles, power storage, and other devices in addition to small portable devices.
[0003] Lithium ion batteries currently available on the market use electrolytes containing flammable organic solvents. On the other hand, lithium ion batteries in which the electrolyte is changed to a solid electrolyte and the battery is made all-solid (hereinafter also referred to as all-solid-state lithium ion batteries) do not use flammable organic solvents in the battery, and therefore are considered to be superior in terms of manufacturing cost and productivity, with simplified safety devices. As a solid electrolyte material used for such solid electrolytes, for example, a sulfide-based solid electrolyte material is known.
[0004] For example, in Patent Document 1 (JP 2016-27545 A), a peak is observed at 2θ=29.86°±1.00° in X-ray diffraction measurement using CuKα radiation, and Li 2y+3 P.S. 4 A sulfide-based solid electrolyte material is described, which is characterized by having a composition of (0.1≦y≦0.175). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-27545 A Summary of the Invention [Problem to be solved by the invention]
[0006] The sulfide-based inorganic solid electrolyte material as described in Patent Document 1 is generally obtained through a process of vitrifying a raw material inorganic composition containing two or more inorganic compounds serving as raw materials for the inorganic solid electrolyte material by mechanically treating the raw material inorganic composition using a method such as mechanical milling. However, according to the study by the present inventors, it has become clear that the process of vitrifying the raw inorganic composition by mechanical treatment is very time-consuming and has poor productivity. In other words, the manufacturing method of the sulfide-based inorganic solid electrolyte material including the process of vitrifying the raw inorganic composition by mechanical treatment as described above is not suitable for industrial production.
[0007] The present invention has been made in consideration of the above circumstances, and provides a method for producing a sulfide-based inorganic solid electrolyte material that can perform the vitrification step in a shorter time and shorten the production time. [Means for solving the problem]
[0008] The present inventors have conducted extensive research to achieve the above object, and as a result have found that the vitrification process of an inorganic composition can be shortened by using two or more types of grinding balls having different diameters in a specific ratio, thereby completing the present invention.
[0009] According to the present invention, A method for producing a sulfide-based inorganic solid electrolyte material containing Li, P and S as constituent elements, comprising: A preparation step of preparing a raw inorganic composition (A) containing at least lithium sulfide and phosphorus sulfide; a vitrification step of mechanically treating the raw inorganic composition (A) using a ball mill and a group of milling balls consisting of two or more types of milling balls having different diameters, thereby vitrifying the raw inorganic composition (A); Including, The group of grinding balls includes at least a first grinding ball and a second grinding ball having a diameter larger than that of the first grinding ball, The present invention provides a method for producing a sulfide-based inorganic solid electrolyte material, in which the amount of the first grinding balls used is 0.1% by mass or more and 9.9% by mass or less when the total amount of the first grinding balls and the second grinding balls in the group of grinding balls is 100% by mass. Effect of the Invention
[0010] According to the present invention, it is possible to provide a method for producing a sulfide-based inorganic solid electrolyte material, which can perform the vitrification step in a shorter time and shorten the production time. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present invention will be described. Note that a numerical range of "A to B" means A or more and B or less unless otherwise specified.
[0012] First, a method for producing a sulfide-based inorganic solid electrolyte material according to this embodiment will be described. The method for producing a sulfide-based inorganic solid electrolyte material according to this embodiment is a method for producing a sulfide-based inorganic solid electrolyte material containing Li, P and S as constituent elements, and includes at least the following steps (A) and (B). Step (A): A preparation step of preparing a raw inorganic composition (A) containing at least lithium sulfide and phosphorus sulfide. Step (B): A vitrification step of mechanically treating the raw inorganic composition (A) using a ball mill and a group of grinding balls consisting of two or more types of grinding balls having different diameters, thereby vitrifying the raw inorganic composition (A). The ball group includes at least first grinding balls and second grinding balls having a diameter larger than that of the first grinding balls, and when the total amount of the first grinding balls and the second grinding balls in the grinding ball group is taken as 100% by mass, the amount of the first grinding balls used is 0.1% by mass or more and 9.9% by mass or less. The ball mill is, for example, made of a cylindrical container.
[0013] According to the method for producing the sulfide-based inorganic solid electrolyte material of this embodiment, the step of vitrifying the inorganic composition can be shortened compared to conventional production methods, and as a result, the production time of the sulfide-based inorganic solid electrolyte material of this embodiment can be shortened.
[0014] In the method for producing a sulfide-based inorganic solid electrolyte material according to the present embodiment, the amount of the first grinding balls used is 0.1% by mass or more and 9.9% by mass or less, but is preferably 1.0% by mass or more, more preferably 2.0% by mass or more, even more preferably 4.0% by mass or more, even more preferably 5.0% by mass or more, and is preferably 9.5% by mass or less, more preferably 9.0% by mass or less, and even more preferably 8.5% by mass or less. When the amount of the first grinding balls used is within the above range, the process of vitrifying the inorganic composition can be further shortened.
[0015] In the method for producing a sulfide-based inorganic solid electrolyte material according to this embodiment, the diameter of the first grinding balls is preferably 1 mm or more and 25 mm or less, more preferably 2 mm or more and 20 mm or less, and even more preferably 5 mm or more and 10 mm or less, from the viewpoint of promoting particle size reduction, and the diameter of the second grinding balls is preferably 2 mm or more and 50 mm or less, more preferably 10 mm or more and 40 mm or less, and even more preferably 20 mm or more and 30 mm or less, from the viewpoint of strong compressive and shear forces.
[0016] In the method for producing a sulfide-based inorganic solid electrolyte material according to this embodiment, the ratio of the diameter of the second grinding balls to the diameter of the first grinding balls is preferably 1.1 or more and 10.0 or less, more preferably 1.7 or more and 8.0 or less, and even more preferably 2.0 or more and 6.0 or less, from the viewpoint of applying strong compressive and shear forces to the fine particles.
[0017] At least the surface of the grinding balls is preferably made of at least one material selected from ceramic materials and metal materials. Examples of metal materials include centrifugally chilled steel, SUS, Cr-plated SUS, and Cr-plated hardened steel. Furthermore, when at least the surface of the grinding balls according to this embodiment is made of a ceramic material, it is possible to prevent unnecessary metal components originating from the grinding balls from being mixed into the obtained sulfide-based inorganic solid electrolyte material, making it possible to obtain a sulfide-based inorganic solid electrolyte material with even higher purity. Examples of such ceramic materials include stabilized zirconia, alumina, silicon carbide, and silicon nitride.
[0018] The sulfide-based inorganic solid electrolyte material obtained by the method for producing a sulfide-based inorganic solid electrolyte material according to this embodiment contains Li, P and S as constituent elements. In addition, in the sulfide-based inorganic solid electrolyte material according to this embodiment, from the viewpoint of further improving lithium ion conductivity, electrochemical stability, stability in moisture and air, and ease of handling, the molar ratio (Li / P) of the Li content to the P content in the solid electrolyte material is preferably 1.0 to 10.0, more preferably 2.0 to 5.0, even more preferably 2.5 to 4.0, even more preferably 2.8 to 3.6, even more preferably 3.0 to 3.5, even more preferably 3.1 to 3.4, and particularly preferably 3.1 to 3.3. In addition, the molar ratio (S / P) of the S content to the P content is preferably 1.0 to 10.0, more preferably 2.0 to 6.0, even more preferably 3.0 to 5.0, even more preferably 3.5 to 4.5, even more preferably 3.8 to 4.2, even more preferably 3.9 to 4.1, and particularly preferably 4.0. Here, the contents of Li, P, and S in the solid electrolyte material of this embodiment can be determined by, for example, ICP emission spectroscopy or X-ray photoelectron spectroscopy.
[0019] The sulfide-based inorganic solid electrolyte material according to this embodiment can be used in any application requiring lithium ion conductivity. In particular, the sulfide-based inorganic solid electrolyte material according to this embodiment is preferably used in a lithium ion battery. More specifically, it is used in a positive electrode active material layer, a negative electrode active material layer, an electrolyte layer, etc. in a lithium ion battery. Furthermore, the sulfide-based inorganic solid electrolyte material according to this embodiment is preferably used in a positive electrode active material layer, a negative electrode active material layer, a solid electrolyte layer, etc. constituting an all-solid-state lithium ion battery, and is particularly preferably used in a solid electrolyte layer constituting an all-solid-state lithium ion battery. An example of an all-solid-state lithium ion battery using the sulfide-based inorganic solid electrolyte material according to this embodiment is one in which a positive electrode, a solid electrolyte layer, and a negative electrode are laminated in this order.
[0020] Each step will be described in detail below.
[0021] (preparation process) First, a raw material inorganic composition (A) containing at least lithium sulfide and phosphorus sulfide is prepared. The raw material inorganic composition (A) can be obtained, for example, by mixing each raw material in a predetermined molar ratio so that the target sulfide-based inorganic solid electrolyte material has a desired composition ratio. Here, the mixing ratio of each raw material in the raw inorganic composition (A) is adjusted so that the resulting sulfide-based inorganic solid electrolyte material has a desired composition ratio. The method for mixing the raw materials is not particularly limited as long as it can mix the raw materials uniformly. For example, the raw materials can be mixed using a ball mill, a bead mill, a vibration mill, an impact grinding device, a mixer (a pug mixer, a ribbon mixer, a tumbler mixer, a drum mixer, a V-type mixer, etc.), a kneader, a two-shaft kneader, an airflow grinder, etc. The mixing conditions when mixing the raw materials, such as the stirring speed, processing time, temperature, reaction pressure, and gravitational acceleration applied to the mixture, can be appropriately determined depending on the processing amount of the mixture.
[0022] The lithium sulfide used as the raw material is not particularly limited, and commercially available lithium sulfide may be used, or lithium sulfide obtained by reacting lithium hydroxide with hydrogen sulfide may be used. From the viewpoint of obtaining a high-purity sulfide-based inorganic solid electrolyte material and suppressing side reactions, it is preferable to use lithium sulfide with few impurities. In this embodiment, lithium sulfide includes lithium polysulfide. Lithium sulfide includes Li 2 S is preferred.
[0023] The phosphorus sulfide used as the raw material is not particularly limited, and may be any commercially available phosphorus sulfide (e.g., P 2 S 5 , P 4 S 3 , P 4 S 7 , P 4 S 5 From the viewpoint of obtaining a high-purity sulfide-based inorganic solid electrolyte material and suppressing side reactions, it is preferable to use phosphorus sulfide with few impurities. 2 S 5 is preferred.
[0024] Lithium nitride may also be used as a raw material. Here, the nitrogen in lithium nitride is N 2 Therefore, by using lithium nitride as the raw inorganic compound, it is possible to increase only the Li composition in a sulfide-based inorganic solid electrolyte material that contains Li, P, and S as constituent elements. The lithium nitride according to the present embodiment is not particularly limited, and may be any commercially available lithium nitride (e.g., Li 3 N, etc.) may be used, or for example, lithium nitride obtained by reacting metallic lithium (for example, Li foil) with nitrogen gas may be used. From the viewpoint of obtaining a high-purity solid electrolyte material and suppressing side reactions, it is preferable to use lithium nitride with few impurities.
[0025] (Vitrification process) Next, the raw inorganic composition (A) is mechanically treated using a ball mill and a group of milling balls consisting of two or more types of milling balls with different diameters, thereby vitrifying the raw inorganic composition (A). That is, the raw materials lithium sulfide and phosphorus sulfide are vitrified while undergoing a chemical reaction, thereby obtaining a sulfide-based inorganic solid electrolyte material in a glassy state. The mechanical treatment herein is a treatment in which two or more inorganic compounds are mechanically collided with each other to cause a chemical reaction and thereby vitrification, and examples thereof include mechanochemical treatment. Furthermore, from the viewpoint of easily realizing an environment in which moisture and oxygen are removed to a high degree in the vitrification step, the mechanical treatment is preferably carried out in a dry manner, and a dry mechanochemical treatment is more preferable. By using the mechanochemical treatment, the raw materials can be mixed while being pulverized into fine particles, so that the contact area of the raw materials can be increased, thereby accelerating the reaction of the raw materials, and the sulfide-based inorganic solid electrolyte material according to the present embodiment can be obtained more efficiently.
[0026] Here, the mechanochemical treatment is a method of vitrifying a target composition while applying mechanical energy such as shear force, collision force, or centrifugal force. In the method for producing a sulfide-based inorganic solid electrolyte material according to the present embodiment, a ball mill is used as an apparatus for vitrifying the composition by the mechanochemical treatment.
[0027] In addition, the mechanochemical treatment is preferably carried out in an inert atmosphere, which can suppress reactions between the sulfide-based inorganic solid electrolyte material and water vapor, oxygen, and the like. The inert atmosphere means a vacuum atmosphere or an inert gas atmosphere. In the inert atmosphere, the dew point is preferably -50°C or less, more preferably -60°C or less, to avoid contact with moisture. The inert gas atmosphere means an atmosphere of an inert gas such as argon gas, helium gas, or nitrogen gas. These inert gases are preferably as high in purity as possible to prevent impurities from being mixed into the product. The method of introducing the inert gas into the mixed system is not particularly limited as long as the mixed system is filled with an inert gas atmosphere, and examples of the method include a method of purging the inert gas and a method of continuously introducing a constant amount of the inert gas.
[0028] The mixing conditions such as the rotation speed, treatment time, temperature, reaction pressure, and gravitational acceleration applied to the raw inorganic composition (A) when mechanically treating the raw inorganic composition (A) can be appropriately determined depending on the type and treatment amount of the raw inorganic composition (A). In general, the faster the rotation speed, the faster the glass production rate, and the longer the treatment time, the higher the conversion rate to glass. Usually, when X-ray diffraction analysis is performed using CuKα radiation as a radiation source, if the diffraction peak derived from the raw material disappears or decreases, it can be determined that the raw material inorganic composition (A) has been vitrified and the desired sulfide-based inorganic solid electrolyte material has been obtained.
[0029] Here, in the step of vitrifying the raw inorganic composition (A), the lithium ion conductivity measured by the AC impedance method under the measurement conditions of 27.0° C., an applied voltage of 10 mV, and a measurement frequency range of 0.1 Hz to 7 MHz is 0.8×10 -4 S cm -1 More than 1.0×10 -4 S cm -1 It is preferable to carry out the mechanical treatment until the above-mentioned temperature is reached, whereby a sulfide-based inorganic solid electrolyte material having even more excellent lithium ion conductivity can be obtained.
[0030] (crystallization process) In the method for producing a sulfide-based inorganic solid electrolyte material according to the present embodiment, from the viewpoint of further improving the lithium ion conductivity of the obtained sulfide-based inorganic solid electrolyte material, it is preferable to further carry out a crystallization step of heating the obtained sulfide-based inorganic solid electrolyte material (hereinafter, the sulfide-based inorganic solid electrolyte material in a glass state after the vitrification step is also referred to as inorganic composition (B)) to crystallize at least a part of the inorganic composition (B). By heating the obtained inorganic composition (B), at least a part of the inorganic composition (B) is crystallized to obtain a sulfide-based inorganic solid electrolyte material in a glass ceramic state (also called crystallized glass). By doing so, for example, a sulfide-based inorganic solid electrolyte material having even better lithium ion conductivity can be obtained. That is, the sulfide-based inorganic solid electrolyte material according to this embodiment is preferably in a glass ceramic state (crystallized glass state) because it has excellent lithium ion conductivity.
[0031] The temperature at which the inorganic composition (B) is heated is not particularly limited as long as it is a temperature at which crystallization can be sufficiently promoted. For example, from the viewpoint of effectively promoting crystallization while suppressing thermal decomposition of the inorganic composition (B), the temperature is preferably in the range of 220°C or higher and 500°C or lower, preferably in the range of 250°C or higher and 400°C or lower, more preferably in the range of 260°C or higher and 350°C or lower, and even more preferably in the range of 270°C or higher and 350°C or lower. The time for heating the inorganic composition (B) is not particularly limited as long as it is a time that can obtain a sulfide-based inorganic solid electrolyte material in a desired glass ceramic state, but is, for example, in the range of 1 minute to 24 hours, preferably in the range of 0.5 hours to 8 hours, and more preferably in the range of 1 hour to 3 hours. The method of heating is not particularly limited, but for example, a method using a calciner can be mentioned. The conditions such as temperature and time during such heating can be appropriately adjusted to optimize the properties of the sulfide-based inorganic solid electrolyte material.
[0032] Moreover, the inorganic composition (B) is preferably heated, for example, in an inert gas atmosphere, which can prevent deterioration (for example, oxidation) of the inorganic composition (B). Examples of the inert gas used when heating the inorganic composition (B) include argon gas, helium gas, and nitrogen gas. In order to prevent impurities from being mixed into the product, it is preferable that these inert gases have a high purity, and in order to avoid contact with moisture, it is preferable that the dew point is -50°C or less, and particularly preferably -60°C or less. The method of introducing the inert gas into the mixed system is not particularly limited as long as the mixed system is filled with an inert gas atmosphere, and examples of the method include a method of purging the inert gas and a method of continuously introducing a constant amount of the inert gas.
[0033] (Heating process) In the method for producing a sulfide-based inorganic solid electrolyte material according to this embodiment, a step of heating the raw inorganic composition (A) prepared in the preparation step may be further carried out between the preparation step and the vitrification step. That is, the above-mentioned vitrification step may be carried out on the raw inorganic composition (A) that has been subjected to a heat treatment. By carrying out the heating step before the vitrification step, the step of vitrifying the raw inorganic composition (A) can be further shortened, and as a result, the production time of the sulfide-based inorganic solid electrolyte material can be further shortened. Although the reason for this is not clear, the following reason is presumed. First, an inorganic composition in a glassy state is in a metastable state. On the other hand, an inorganic composition in a crystalline state is in a stable state. In addition, when an inorganic composition containing two or more inorganic compounds is heated, energy equal to or greater than the activation energy can be easily applied, and the inorganic composition in a crystalline state, which is in a low energy state, can be obtained in a short time with the release of energy. Furthermore, since the free energy of the stable state and the free energy of the metastable state are close, it is possible to change from the stable crystalline state to the metastable glass state with less energy. For the above reasons, it is believed that by carrying out a step of heating the raw inorganic composition (A) prior to the step of vitrifying the raw inorganic composition (A) and converting the raw inorganic composition (A) into a stable crystalline state in advance, it is possible to convert the raw inorganic composition (A) into a metastable glassy state with less energy, and thus significantly shorten the step of vitrifying the raw inorganic composition (A).
[0034] The temperature at which the raw inorganic composition (A) is heated is not particularly limited, and can be appropriately set depending on the sulfide-based inorganic solid electrolyte material to be produced. For example, the heating temperature is preferably within the range of 200°C or higher and 400°C or lower, and more preferably within the range of 220°C or higher and 300°C or lower.
[0035] The time for heating the raw inorganic composition (A) is not particularly limited, but is, for example, within the range of 1 minute to 24 hours, preferably 0.1 hours to 10 hours. The method for heating is not particularly limited, but for example, a method using a calciner can be mentioned. The conditions such as temperature and time during such heating can be appropriately adjusted to optimize the properties of the sulfide-based inorganic solid electrolyte material according to this embodiment.
[0036] Whether the raw inorganic composition (A) has crystallized can be determined, for example, by whether a new crystal peak is generated in a spectrum obtained by X-ray diffraction using CuKα radiation as a radiation source.
[0037] (Crushing, classifying, or granulating process) In the method for producing a sulfide-based inorganic solid electrolyte material according to this embodiment, a step of pulverizing, classifying, or granulating the obtained sulfide-based inorganic solid electrolyte material may be further performed as necessary. For example, a sulfide-based inorganic solid electrolyte material having a desired particle size can be obtained by pulverizing to obtain fine particles, and then adjusting the particle size by a classification operation or a granulation operation. The above-mentioned pulverizing method is not particularly limited, and known pulverizing methods such as a mixer, airflow pulverization, a mortar, a rotary mill, and a coffee mill can be used. The above-mentioned classification method is also not particularly limited, and known methods such as a sieve can be used. The pulverization or classification is preferably carried out in an inert gas atmosphere or a vacuum atmosphere, since this can prevent contact with moisture in the air.
[0038] In order to obtain the sulfide-based inorganic solid electrolyte material according to this embodiment, it is important to appropriately adjust each of the above steps. However, the method for producing the sulfide-based inorganic solid electrolyte material according to this embodiment is not limited to the above method, and the sulfide-based inorganic solid electrolyte material according to this embodiment can be obtained by appropriately adjusting various conditions.
[0039] Although the embodiments of the present invention have been described above, these are merely examples of the present invention, and various configurations other than those described above can also be adopted. The present invention is not limited to the above-described embodiment, and modifications and improvements within the scope of the present invention that can achieve the object of the present invention are included in the present invention. EXAMPLES
[0040] EXAMPLES Hereinafter, the present invention will be described with reference to examples and comparative examples, but the present invention is not limited to these.
[0041] <Evaluation method> First, the evaluation methods in the following Examples and Comparative Examples will be described.
[0042] (1) Measurement of lithium ion conductivity The lithium ion conductivity of the sulfide-based inorganic solid electrolyte materials obtained in the examples and comparative examples was measured by an AC impedance method. The lithium ion conductivity was measured using a potentiostat / galvanostat SP-300 manufactured by Biologic Corp. The sample size was 9.5 mm in diameter and 1.2 to 2.0 mm in thickness, and the measurement conditions were an applied voltage of 10 mV, a measurement temperature of 27.0°C, a measurement frequency range of 0.1 Hz to 7 MHz, and a Li foil electrode. Here, as the sample for measuring lithium ion conductivity, a plate-shaped sulfide-based inorganic solid electrolyte material having a diameter of 9.5 mm and a thickness of 1.2 to 2.0 mm was used, which was obtained by pressing 150 mg of the powdered sulfide-based inorganic solid electrolyte material obtained in the examples and comparative examples at 270 MPa for 10 minutes using a pressing device.
[0043] <Example 1> A sulfide-based inorganic solid electrolyte material was prepared by the following procedure. The raw materials are Li 2 S (manufactured by Furukawa Co., Ltd., purity 99.9%) and P 2 S 5 (Kanto Chemical Co., Ltd.) was used. Then, in an argon glove box, Li 2 S powder and P 2 S 5 Powder (Li 2 S:P 2 S 5 =80:20 (molar ratio)) were precisely weighed out, and all the powders were mixed for 10 minutes in an agate mortar to obtain a mixed powder (raw inorganic composition (A)). Next, 300 g of the obtained mixed powder and a ZrO 2 500g of ZrO ball and 25mm diameter 2 Then, 7,000 g of aluminum balls were added to the cylindrical container, and the cylindrical container was sealed. The cylindrical container was then attached to a ball mill, and the mixture was pulverized and mixed (mechanochemical treatment) at a rotation speed of 100 rpm for 600 hours to obtain a glass-state sulfide-based inorganic solid electrolyte material (Li 12 P 3 S 13.5 ) was obtained. The lithium ion conductivity of each of the obtained glass-state sulfide-based inorganic solid electrolyte materials was measured. The results are shown in Table 1.
[0044] <Comparative Example 1> A glassy sulfide-based inorganic solid electrolyte material was prepared in the same manner as in Example 1, except that the conditions of the mechanochemical treatment using a ball mill were changed as shown in Table 1, and the lithium ion conductivity of the obtained glassy sulfide-based inorganic solid electrolyte material was measured. The obtained results are shown in Table 1.
[0045] <Example 2> A sulfide-based inorganic solid electrolyte material was prepared by the following procedure. The raw materials are Li 2 S (manufactured by Furukawa Co., Ltd., purity 99.9%), P 2 S 5 (Kanto Chemical Co., Ltd.) and Li 3 N (manufactured by Furukawa Co., Ltd.) was used. Then, in an argon glove box, Li 2 S powder and P 2 S 5 Powder and Li 3 N powder (Li 2 S:P 2 S 5 :Li 3 N=27:9:2 (molar ratio)) were precisely weighed out, and all the powders were mixed for 10 minutes in an agate mortar to obtain a mixed powder (raw inorganic composition (A)). Next, 300 g of the mixed powder obtained and a ZrO 2 500g of ZrO ball and 25mm diameter 2 The cylindrical container was then sealed. The cylindrical container was then attached to a ball mill and pulverized and mixed (mechanochemical treatment) at a rotation speed of 100 rpm for 750 hours to obtain a glass-state sulfide-based inorganic solid electrolyte material (Li 10 P 3 S 12 ) was obtained. The lithium ion conductivity of each of the obtained glass-state sulfide-based inorganic solid electrolyte materials was measured. The results are shown in Table 1.
[0046] <Example 3 and Comparative Examples 2 to 3> A glassy sulfide-based inorganic solid electrolyte material was prepared in the same manner as in Example 2, except that the conditions of the mechanochemical treatment using a ball mill were changed as shown in Table 1, and the lithium ion conductivity of the obtained glassy sulfide-based inorganic solid electrolyte material was measured. The obtained results are shown in Table 1.
[0047] [Table 1]
[0048] When comparing sulfide-based inorganic solid electrolyte materials of the same type, it can be seen that the manufacturing method of the sulfide-based inorganic solid electrolyte material of the embodiment produces a sulfide-based inorganic solid electrolyte material with higher ionic conductivity in a shorter time. From the above, it can be understood that according to the method for producing a sulfide-based inorganic solid electrolyte material according to this embodiment, the inorganic composition can be vitrified in a shorter time, and the production time can be shortened.
Claims
1. A method for producing a sulfide-based inorganic solid electrolyte material containing Li, P and S as constituent elements, comprising: A preparation step of preparing a raw material inorganic composition (A) containing at least lithium sulfide and phosphorus sulfide; a vitrification step of mechanically treating the raw inorganic composition (A) using a ball mill and a group of milling balls consisting of two or more types of milling balls having different diameters, thereby vitrifying the raw inorganic composition (A); Including, The group of grinding balls includes at least a first grinding ball and a second grinding ball having a diameter larger than that of the first grinding ball, When the total amount of the first and second crushing balls in the crushing ball group is taken as 100% by mass, the amount of the first crushing balls used is 4.0% by mass or more and 9.9% by mass or less; A method for producing a sulfide-based inorganic solid electrolyte material, wherein a ratio of a diameter of the second crushing balls to a diameter of the first crushing balls is 1.7 or more.
2. The method for producing a sulfide-based inorganic solid electrolyte material according to claim 1, The diameter of the first grinding ball is 1 mm or more and 10 mm or less, The method for producing a sulfide-based inorganic solid electrolyte material, wherein the second crushing balls have a diameter of 20 mm or more and 50 mm or less.
3. The method for producing a sulfide-based inorganic solid electrolyte material according to claim 1 or 2, A method for producing a sulfide-based inorganic solid electrolyte material, wherein a ratio of a diameter of the second crushing balls to a diameter of the first crushing balls is 2.0 or more and 10.0 or less.
4. The method for producing a sulfide-based inorganic solid electrolyte material according to any one of claims 1 to 3, The method for producing a sulfide-based inorganic solid electrolyte material, wherein the mechanical treatment in the vitrification step includes a mechanochemical treatment.
5. The method for producing a sulfide-based inorganic solid electrolyte material according to any one of claims 1 to 4, A method for producing a sulfide-based inorganic solid electrolyte material, wherein the mechanical treatment in the vitrification step is performed by a dry method.
6. The method for producing a sulfide-based inorganic solid electrolyte material according to any one of claims 1 to 5, The method for producing a sulfide-based inorganic solid electrolyte material further comprises, after the vitrification step, a crystallization step of heating the obtained inorganic composition (B) to crystallize at least a part of the inorganic composition (B).
Citation Information
Patent Citations
Pulverizing method of powder particle and modifying method of particle
JP1997253517A
Method for operating horizontal ultrafine particle mill
JP1998137609A
Method for producing intercalation compound
JP2006265073A
Method of producing sulfide-based solid electrolyte
JP2010090003A
Method of producing sulfide solid electrolyte