Rubber composition and tire
A rubber composition with a high silica content and hydrogenated resin enhances wet grip and reduces rolling resistance in tires by optimizing compatibility and elastic modulus, addressing the balance between these performance metrics.
Patent Information
- Application Number
- JP2021565629
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-19
- Filing Date
- 2020-12-16
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2040-12-16
AI Technical Summary
Existing rubber compositions for tires struggle to achieve a balance between improved wet grip properties and reduced rolling resistance, with conventional formulations often compromising on one or both performance metrics.
A rubber composition comprising a rubber component, a filler, and a hydrogenated resin with a high softening point and specific molecular weight, along with a high silica content, is used to enhance compatibility and control the elastic modulus, thereby improving wet grip and reducing rolling resistance.
The composition results in tires with excellent wet grip properties and low rolling resistance, maintaining optimal handling properties and wear resistance.
Smart Images

Figure 0007566782000001 
Figure 0007566782000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber composition and a tire. [Background technology]
[0002] From the viewpoint of improving the safety of vehicles, various studies have been made to improve the braking performance and driving performance of tires not only on dry road surfaces but also on various road surfaces such as wet road surfaces and snowy and icy road surfaces. For example, as a rubber composition capable of producing a tread rubber having high braking performance on dry road surfaces and also high braking performance on wet road surfaces such as manholes that are slippery compared to asphalt, a rubber composition has been disclosed that is made by blending a rubber component (A) containing 70% by mass or more of natural rubber, and blending 5 to 50 parts by mass of at least one thermoplastic resin (B) selected from C5 resin, C5-C9 resin, C9 resin, terpene resin, terpene-aromatic compound resin, rosin resin, dicyclopentadiene resin, and alkylphenol resin, and 20 to 120 parts by mass of a filler (C) containing silica, relative to 100 parts by mass of the rubber component, in which the silica content in the filler (C) is 50 to 100% by mass (see, for example, Patent Document 1).
[0003] In addition, as a rubber composition for tires that can improve grip performance on dry road surfaces without impairing grip performance on wet road surfaces, a rubber composition for tires has been disclosed that contains 100 parts by mass of a diene rubber component containing 70 parts by mass or more of styrene-butadiene rubber having a styrene content of 20 to 60% by mass in the rubber component, and that contains 50 to 300 parts by mass of silica, 0 to 150 parts by mass of an inorganic agent represented by the general formula mM1·xSiOy·zH2O, and 0 to 150 parts by mass of carbon black, such that the total amount of silica and the inorganic agent is 200 to 350 parts by mass and the total amount of silica, the inorganic agent, and the carbon black is 200 to 350 parts by mass, contains a softener in an amount of 70% by mass or more with respect to the total filler amount, and contains 5 to 60 parts by mass of at least one resin having a softening point of 145°C or less (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2015 / 079703 [Patent Document 2] JP 2008-184505 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the rubber compositions disclosed in Patent Documents 1 and 2 are required to further improve the balance between improved wet grip performance and reduced rolling resistance. An object of the present invention is to provide a tire having excellent wet grip properties and low rolling resistance, and a rubber composition from which the tire and a vulcanized rubber having excellent handling properties can be produced, and an object of the present invention is to achieve the object. [Means for solving the problem]
[0006] <1> A rubber composition comprising: a rubber component; 40 to 125 parts by mass of a filler relative to 100 parts by mass of the rubber component; and 5 to 50 parts by mass of a hydrogenated resin having a softening point higher than 110°C and a weight average molecular weight in terms of polystyrene of 200 to 1200 g / mol relative to 100 parts by mass of the rubber component.
[0007] <2> The rubber component contains styrene-butadiene rubber. <1> The rubber composition according to claim 1. <3> The rubber component contains a rubber having an isoprene skeleton. <1> or <2> The rubber composition according to claim 1. <4> The filler contains silica, and the content of the silica in the filler is 80 mass % or more. <1> ~ <3> The rubber composition according to any one of the above. <5> The hydrogenated resin is at least one selected from the group consisting of hydrogenated C5 resins, hydrogenated C5-C9 resins, and hydrogenated dicyclopentadiene resins. <1> ~ <4> The rubber composition according to any one of the above. <6> The styrene-butadiene rubber has no modifying group at the end of the main chain. <2> ~ <5> The rubber composition according to any one of the above.
[0008] <7> <1> ~ <6> A tire using the rubber composition according to any one of claims 1 to 5. Effect of the Invention
[0009] According to the present invention, it is possible to provide a tire having excellent wet grip performance and low rolling resistance, and a rubber composition from which the tire and a vulcanized rubber having excellent handling properties can be produced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] <Rubber composition> The rubber composition of the present invention includes a rubber component, 40 to 125 parts by mass of a filler relative to 100 parts by mass of the rubber component, and 5 to 50 parts by mass of a hydrogenated resin having a softening point higher than 110°C and a weight average molecular weight in terms of polystyrene of 200 to 1200 g / mol relative to 100 parts by mass of the rubber component. "A hydrogenated resin having a softening point of more than 110° C. and a weight average molecular weight of 200 to 1200 g / mol in terms of polystyrene" is sometimes referred to as "the hydrogenated resin of the present invention."
[0011] In conventional technology, wet grip performance was improved by using inorganic fillers such as silica. However, such fillers have the problem of increasing energy loss. In addition, studies have been conducted to provide rubber compositions for tire treads that have an excellent balance between wet grip performance and low rolling resistance without impairing the abrasion resistance of tires by blending rubbers with different glass transition temperatures (Tg), but there were still some shortcomings in terms of low loss performance, abrasion resistance, etc. In recent years, various studies have been conducted, such as compounding with a larger amount of thermoplastic resin in the rubber composition, compounding with a higher silica ratio in the filler, compounding with modified polymers that highly disperse silica, etc., but there are limits to resolving the tradeoffs. In particular, the technology of compounding a large amount of softeners, such as thermoplastic resins, has the problem of a decrease in the elastic modulus of rubber. In contrast, since the rubber composition of the present invention has the above-mentioned configuration, the vulcanized rubber obtained from the rubber composition of the present invention has excellent handling properties, and the tire obtained from the rubber composition of the present invention has excellent wet grip properties and low rolling resistance.
[0012] The reason for this is unclear, but is presumed to be due to the following reasons. The hydrogenated resin of the present invention has a polystyrene-equivalent weight average molecular weight of 1200 or less, and is compatible with rubber components due to its low molecular weight, and since the hydrogenated resin of the present invention has a high softening point, it is believed to reinforce the rubber components and reduce the rolling resistance of tires without significantly decreasing or increasing the elastic modulus of the vulcanized rubber. At the same time, the hydrogenated resin of the present invention, due to its compatibility, is believed to be able to impart the flexibility required for road grip to tires, and to improve grip on slippery wet roads, i.e., wet grip. In addition, since the rubber composition contains the hydrogenated resin of the present invention, the elastic modulus (E') of the vulcanized rubber can be controlled within a range that is neither too large nor too small, and it is believed that the handleability of the vulcanized rubber is also excellent. From the above, it is considered that a tire obtained from the rubber composition of the present invention has excellent wet grip performance and low rolling resistance. The rubber composition and tire of the present invention will be described in detail below.
[0013] [Rubber component] The rubber composition of the present invention contains a rubber component. The rubber component is not particularly limited, and examples of the rubber that can be used include natural rubber (NR), as well as synthetic rubbers such as styrene butadiene rubber (SBR), butadiene rubber (BR), isoprene rubber (IR), chloroprene rubber, butyl rubber (IIR), halogenated butyl rubber, ethylene-propylene rubber (EPR, EPDM), fluororubber, silicone rubber, and urethane rubber. Among these, it is preferable to use diene rubbers such as natural rubber (NR), styrene butadiene rubber (SBR), butadiene rubber (BR), and isoprene rubber (IR). The rubber component is preferably an unmodified rubber. It is preferable that the styrene-butadiene rubber does not contain a modified styrene-butadiene rubber. It is preferable that the styrene-butadiene rubber does not have a modifying group at the molecular end (particularly, the end of the main chain). The rubber component may be used alone or in combination of two or more kinds.
[0014] The rubber component preferably contains a rubber having an isoprene skeleton from the viewpoints of improving the mechanical strength of the vulcanized rubber and enhancing the abrasion resistance, tear strength, etc. Also, from the viewpoints of improving the wet grip performance of the tire and further reducing the rolling resistance, the rubber component preferably contains a styrene-butadiene rubber.
[0015] (rubber with isoprene structure) By including a rubber having an isoprene skeleton in the rubber component, the breaking strength of the vulcanized rubber can be increased, which results in lower rolling resistance of the tire and excellent abrasion resistance, tear strength, etc. of the vulcanized rubber. Examples of rubbers having an isoprene skeleton include natural rubber (NR) and polyisoprene rubber (IR). The content of the rubber having an isoprene skeleton in the rubber component is preferably 10 to 90 mass %, more preferably 20 to 80 mass %, and even more preferably 30 to 70 mass %, from the viewpoints of lowering the rolling resistance of the tire and improving the abrasion resistance, tear strength, etc. of the vulcanized rubber.
[0016] [Filler] The rubber composition of the present invention contains 40 to 125 parts by mass of a filler based on 100 parts by mass of the rubber component. If the content of the filler in the rubber composition is less than 40 parts by mass per 100 parts by mass of the rubber component, the tire will not be sufficiently reinforced, and if it exceeds 125 parts by mass, the rolling resistance cannot be reduced and the elastic modulus of the tire will become too high, resulting in poor wet grip performance. From the viewpoint of improving wet grip performance, the content of the filler in the rubber composition is preferably 45 parts by mass or more, more preferably 50 parts by mass or more, and even more preferably 55 parts by mass or more, per 100 parts by mass of the rubber component. Also, from the viewpoint of lowering the rolling resistance, the content of the filler in the rubber composition is preferably 110 parts by mass or less, more preferably 100 parts by mass or less, and even more preferably 90 parts by mass or less, per 100 parts by mass of the rubber component. The filler is not particularly limited, and examples thereof include inorganic fillers such as silica, clay, talc, calcium carbonate, aluminum hydroxide, and carbon black. Among them, the filler is preferably silica or carbon black, and more preferably contains at least silica.
[0017] (silica) Examples of silica include wet silica (hydrated silicic acid), dry silica (anhydrous silicic acid), calcium silicate, aluminum silicate, etc., and among these, wet silica is preferred. These silicas may be used alone or in combination of two or more. Silica has a nitrogen adsorption specific surface area (BET method) of 130m 2 / g or more 330m 2 It is preferable that the molecular weight is less than 1 / g. The nitrogen adsorption specific surface area of silica (BET method) is 130m 2 / g or more, the tire can be sufficiently reinforced and the rolling resistance can be further reduced. In addition, the nitrogen adsorption specific surface area of silica (BET method) is 330 m 2 / g, the elastic modulus of the tire is not excessively increased, and the tire has excellent wet grip properties. From the viewpoint of lowering the rolling resistance and improving the abrasion resistance and tear strength of the tire, the nitrogen adsorption specific surface area of silica (BET method) is set at 180m 2 / g or more is more preferable, and 190m 2 From the viewpoint of further improving the wet grip performance, the nitrogen adsorption specific surface area (BET method) of silica is preferably 300 m 2 / g or less is more preferable, 2 / g or less is more preferable, and 2 It is more preferable that the molecular weight is not more than 1 / g.
[0018] From the viewpoint of improving the mechanical strength of the tire and further reducing the rolling resistance, the content of silica in the filler is preferably 80 mass % or more, more preferably 85 mass % or more, and even more preferably 90 mass % or more. From the viewpoints of improving the mechanical strength of the tire and further improving the wet grip performance, the content of silica in the rubber composition is preferably 30 parts by mass or more, more preferably 35 parts by mass or more, and even more preferably 40 parts by mass or more, per 100 parts by mass of the rubber component. From the viewpoints of further reducing the rolling resistance, the content of silica in the rubber composition is preferably 90 parts by mass or less, more preferably 85 parts by mass or less, and even more preferably 80 parts by mass or less, per 100 parts by mass of the rubber component.
[0019] (Carbon Black) The filler preferably further contains carbon black, provided that the carbon black is contained in such a range that the silica content in the filler is 80 mass % or more. Carbon black reinforces the vulcanized rubber and improves the abrasion resistance of the vulcanized rubber. The carbon black is not particularly limited, and examples thereof include GPF, FEF, HAF, ISAF, and SAF grade carbon black. These carbon blacks may be used alone or in combination of two or more.
[0020] From the viewpoint of improving the abrasion resistance of the vulcanized rubber, the content of carbon black in the rubber composition is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more, per 100 parts by mass of the rubber component. Also, from the viewpoint of maintaining the low loss property of the vulcanized rubber, the content of carbon black in the rubber composition is preferably 15 parts by mass or less, more preferably 12 parts by mass or less, and even more preferably 9 parts by mass or less, per 100 parts by mass of the rubber component.
[0021] [Hydrogenated Resin] The rubber composition contains a hydrogenated resin having a softening point higher than 110° C. and a weight average molecular weight in terms of polystyrene of 200 to 1200 g / mol. The content of the hydrogenated resin in the rubber composition is 5 to 50 parts by mass per 100 parts by mass of the rubber component. If the softening point of the hydrogenated resin is 110°C or less, the wet performance cannot be improved. From the viewpoint of improving the wet performance, the softening point of the hydrogenated resin is preferably 115°C or more, more preferably 118°C or more, even more preferably 121°C or more, even more preferably 123°C or more, even more preferably 125°C or more, even more preferably 127°C or more, even more preferably 128°C or more, and even more preferably 129°C or more. In addition, from the viewpoint of suppressing an increase in not only tan δ at 0°C but also tan δ at 50°C, which is the rolling region, the softening point of the hydrogenated resin is preferably 145°C or less, preferably 143°C or less, more preferably 140°C or less, more preferably 136°C or less, even more preferably 135°C or less, and even more preferably 133°C or less.
[0022] If the weight-average molecular weight of the hydrogenated resin in terms of polystyrene is less than 200 g / mol, the hydrogenated resin will precipitate from the tire and the effects of the hydrogenated resin will not be fully exerted. On the other hand, if it exceeds 1,200 g / mol, the hydrogenated resin will not be compatible with the rubber component. From the viewpoint of suppressing the precipitation of the hydrogenated resin from the tire and suppressing the deterioration of the tire appearance, the weight average molecular weight of the hydrogenated resin in terms of polystyrene is preferably 300 g / mol or more, more preferably 500 g / mol or more, more preferably 700 g / mol or more, and even more preferably 750 g / mol or more. From the viewpoint of increasing the compatibility of the hydrogenated resin with the rubber component and further increasing the effect of the hydrogenated resin, the weight average molecular weight of the hydrogenated resin in terms of polystyrene is preferably 1150 g / mol or less, more preferably 1100 g / mol or less, even more preferably 1050 g / mol or less, even more preferably 950 g / mol or less, even more preferably 930 g / mol or less, and even more preferably 900 g / mol or less. The hydrogenated resin is a high-softening point hydrocarbon resin prepared by polymerizing a mixture of hydrocarbon fractions having carbon numbers of C5 or more obtained by steam cracking of propane and ethane using a Friedel-Crafts catalyst.
[0023] When the content of the hydrogenated resin in the rubber composition is less than 5 parts by mass per 100 parts by mass of the rubber component, the effect of the hydrogenated resin cannot be exerted. When the content of the hydrogenated resin exceeds 50 parts by mass, the hydrogenated resin precipitates from the tire, and the effect of the hydrogenated resin cannot be fully exerted. From the viewpoint of further enhancing the effect of the hydrogenated resin, the content of the hydrogenated resin in the rubber composition is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 20 parts by mass or more, per 100 parts by mass of the rubber component. Also, from the viewpoint of suppressing precipitation of the hydrogenated resin from the tire and suppressing deterioration of the tire appearance, the content of the hydrogenated resin in the rubber composition is preferably 47 parts by mass or less, more preferably 43 parts by mass or less, and even more preferably 40 parts by mass or less, per 100 parts by mass of the rubber component.
[0024] The hydrogenated resin means a resin obtained by reducing and hydrogenating a resin. Examples of resins that can be used as raw materials for hydrogenated resins include C5 resins, C5-C9 resins, C9 resins, terpene resins, dicyclopentadiene resins, and terpene-aromatic compound resins. These resins may be used alone or in combination of two or more.
[0025] Examples of C5 resins include aliphatic petroleum resins obtained by (co)polymerizing C5 fractions obtained by thermal cracking of naphtha in the petrochemical industry. The C5 fraction usually contains olefinic hydrocarbons such as 1-pentene, 2-pentene, 2-methyl-1-butene, 2-methyl-2-butene, and 3-methyl-1-butene, and diolefinic hydrocarbons such as 2-methyl-1,3-butadiene, 1,2-pentadiene, 1,3-pentadiene, and 3-methyl-1,2-butadiene, etc. Note that commercially available products can be used as the C5 resin.
[0026] C5-C9 resin refers to C5-C9 synthetic petroleum resin. Examples of C5-C9 resin include petroleum-derived C5-C 11 Examples of such solid polymers include those obtained by polymerizing the fraction using a Friedel-Crafts catalyst such as AlCl3 or BF3. More specifically, examples of such solid polymers include copolymers mainly composed of styrene, vinyltoluene, α-methylstyrene, indene, etc. As the C5-C9 resin, a resin with a small amount of C9 or more components is preferred from the viewpoint of compatibility with the rubber component. Here, "a small amount of C9 or more components" means that the amount of C9 or more components in the total amount of the resin is less than 50 mass%, preferably 40 mass% or less. Commercially available C5-C9 resins can be used.
[0027] Furthermore, the resin that is the raw material for the hydrogenated resin may contain, for example, a resin obtained by copolymerizing a C5 fraction with dicyclopentadiene (DCPD) (C5-DCPD resin). Here, when the dicyclopentadiene-derived component in the total amount of resin is 50 mass% or more, the C5-DCPD-based resin is considered to be included in the dicyclopentadiene-based resin.When the dicyclopentadiene-derived component in the total amount of resin is less than 50 mass%, the C5-DCPD-based resin is considered to be included in the C5-based resin.
[0028] From the viewpoints of increasing the compatibility between the rubber component and the hydrogenated resin, further improving the wet grip performance, and further improving the balance between rolling resistance and handling, the hydrogenated resin is preferably at least one selected from the group consisting of hydrogenated C5 resins, hydrogenated C5-C9 resins, and hydrogenated dicyclopentadiene resins (hydrogenated DCPD resins), more preferably at least one selected from the group consisting of hydrogenated C5 resins and hydrogenated C5-C9 resins, and even more preferably a hydrogenated C5 resin.
[0029] (Silane coupling agent) The rubber composition preferably further contains a silane coupling agent. As the silane coupling agent, any silane coupling agent commonly used in the rubber industry can be used.
[0030] (Various ingredients) The rubber composition of the present invention may contain the above-mentioned rubber component, filler, and hydrogenated resin, as well as various other components commonly used in the rubber industry, as necessary, such as a softener, a resin other than the hydrogenated resin of the present invention, a processability improver, stearic acid, an antioxidant, zinc oxide, a vulcanization accelerator, and a vulcanizing agent, all of which are appropriately selected within ranges not impairing the object of the present invention.
[0031] [Method for producing rubber composition] The method for producing the rubber composition of the present invention is not particularly limited. For example, the rubber composition can be produced by blending the above-mentioned rubber component, silica, and the hydrogenated resin of the present invention with various components appropriately selected as necessary, and kneading, heating, extruding, or the like.
[0032] <Tires> The tire (pneumatic tire) of the present invention is made using the rubber composition of the present invention. As described above, a tire obtained from the rubber composition of the present invention has excellent wet grip properties and low rolling resistance, and therefore the rubber composition of the present invention is suitable for use in the tread portion of a tire.
[0033] Depending on the type and components of the tire to be applied, the tire may be obtained by molding an unvulcanized rubber composition and then vulcanizing it, or by first obtaining a semi-vulcanized rubber from an unvulcanized rubber composition through a pre-vulcanization step or the like, and then molding the semi-vulcanized rubber using the semi-vulcanized rubber, followed by further vulcanization. As the gas to be filled into the tire, in addition to normal air or air with an adjusted oxygen partial pressure, inert gases such as nitrogen, argon, and helium can be used. EXAMPLES
[0034] The present invention will be described in more detail below by way of examples. However, these examples are intended to illustrate the present invention and are not intended to limit the present invention in any way.
[0035] <Preparation of Rubber Composition> The rubber compositions of the Examples and Comparative Examples were prepared by mixing using a normal Banbury mixer according to the compounding recipes shown in Tables 1 and 2. The maximum temperature of the mixture was 170°C. Details of each component in Tables 1 and 2 are as follows.
[0036] [Rubber component] NR: Natural rubber, TSR20 SBR: JSR Corporation, product name "SBR #1500", bound styrene content: 24%
[0037] [Fillers, silane coupling agents] CB: Carbon black, N134, Asahi Carbon Co., Ltd., nitrogen adsorption specific surface area (NSA) = 146 m 2 / g Silica: Tosoh Silica Corporation, product name "Nipsil AQ", nitrogen adsorption specific surface area (BET method) = 205 m 2 / g Silane coupling agent: Evonic, product name "Si69"
[0038] [Softener] (hydrogenated resin) Hydrogenated C5 resin: Eastman Co., product name "Impera E1780" (Non-hydrogenated resin) C9 resin: JXTG Terpen phenol resin: Yasuhara (oil) Oil: Idemitsu Kosan Co., Ltd., product name "Diana Process NH-70S"
[0039] Regarding the softener, the softening point (Ts) and weight average molecular weight (Mw) of each resin are shown in Table 2.
[0040] [Various ingredients] 6C: Antioxidant, N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Nocrac 6C" DM: Vulcanization accelerator, di-2-benzothiazolyl disulfide, manufactured by Sanshin Chemical Industry Co., Ltd., product name "Suncerer DM" NS: Vulcanization accelerator, Nt-butyl-2-benzothiazylsulfenamide, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., product name "Noccela NS" DPG: Vulcanization accelerator, 1,3-diphenylguanidine, Sanshin Chemical Industry Co., Ltd., product name "Suncerer D"
[0041] <Vulcanization of Rubber Composition and Evaluation of Vulcanized Rubber> 1.Rolling resistance The rubber composition was vulcanized at 160°C for 15 minutes to obtain a vulcanized rubber test piece, and the loss tangent (tan δ) of the vulcanized rubber test piece was measured using a viscoelasticity measuring device under the conditions of dynamic strain: 1%, frequency: 52 Hz, and measurement temperature: 50°C. The tan δ of the vulcanized rubber test piece of Comparative Example 3 was set to 100, and the measured values of each Example and Comparative Example were expressed as an index (RR index). The larger the index, the smaller and more favorable the rolling resistance. The results are shown in Table 2.
[0042] 2.Wet grip The rubber composition was vulcanized at 160°C for 15 minutes to obtain a vulcanized rubber test piece, and the loss tangent (tan δ) of the vulcanized rubber test piece was measured using a viscoelasticity measuring device under the conditions of dynamic strain: 1%, frequency: 52 Hz, and measurement temperature: 0°C. The resistance value of Comparative Example 3 was set to 100, and the measured values of each Example and Comparative Example were expressed as an index (Wet index). The larger the index, the larger the resistance value and the more excellent the wet grip performance. The results are shown in Table 2. The acceptable range is 150 or more.
[0043] 3. Handling of vulcanized rubber The rubber composition was vulcanized at 160° C. for 15 minutes to obtain a vulcanized rubber, and the storage modulus (E′) was measured using a viscoelasticity measuring device under conditions of a temperature of 30° C., a dynamic strain of 1%, and a frequency of 52 Hz. The measurement result of the vulcanized rubber of Comparative Example 3 was set to 100, and the E′ index was calculated according to the following formula and is shown in Table 2. E' index = (E' other than Comparative Example 3 / E' of Comparative Example 3) x 100 The handleability of the vulcanized rubber is not excellent if the E' index is too small or too large.
[0044] [Table 1]
[0045] [Table 2]
[0046] From the results of the examples shown in Table 2, it can be seen that by using the compounding composition according to the present invention, the handling property of the vulcanized rubber is excellent, and by using the rubber composition, a tire having excellent wet grip property and low rolling resistance can be obtained. [Industrial Applicability]
[0047] By using the rubber composition of the present invention, a tire having excellent wet grip and low rolling resistance can be obtained. Since the rubber composition of the present invention can be used for tires, the rubber composition of the present invention can be suitably used for producing tires for passenger cars, trucks, buses, etc.
Claims
1. A rubber component, A filler in an amount of 40 to 125 parts by mass per 100 parts by mass of the rubber component; a hydrogenated resin having a softening point higher than 110° C. and a weight average molecular weight in terms of polystyrene of 200 to 1200 g / mol, and the hydrogenated resin is present in an amount of 5 to 50 parts by mass per 100 parts by mass of the rubber component; The rubber component contains a styrene-butadiene rubber and a rubber having an isoprene skeleton, The rubber composition, wherein the hydrogenated resin is at least one selected from the group consisting of hydrogenated C 5 resins, hydrogenated C 5 -C 9 resins, and hydrogenated dicyclopentadiene resins.
2. The rubber composition according to claim 1 , wherein the filler contains silica, and the content of the silica in the filler is 80 mass % or more.
3. 3. The rubber composition according to claim 1, wherein the styrene-butadiene rubber has no modifying group at an end of the main chain.
4. A tire using the rubber composition according to any one of claims 1 to 3.
Citation Information
Patent Citations
Rubber composition for tire and pneumatic tire using the same
JP2008174696A
Rubber composition for tire, and pneumatic tire using the same
JP2008184505A
Method for manufacturing pneumatic tire
JP2013099898A
Adhesive composition, and conductive adhesive sheet