Method for producing laminate having clear layer, laminate obtained by the method, method for producing composite coating film, composite coating film obtained by the method, method for producing molded article using the same, molded article, and clear layer obtained from the above laminate

The described method addresses environmental and quality issues in automotive coatings by using a solvent-based clear paint composition with a cover material to capture and pass solvents, resulting in a high-quality clear layer with improved resistance and smoothness.

JP7567046B2Active Publication Date: 2024-10-15BASF COATINGS JAPAN +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023516371
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-04-22
Filing Date
2022-03-25
Publication Date
2024-10-15
Estimated Expiration
2042-03-25

AI Technical Summary

Technical Problem

Conventional coating methods for automotive bodies face environmental burdens due to volatile organic compounds (VOCs), require long curing times, and struggle to produce a clear layer with consistent quality, weather resistance, and scratch resistance, especially for luxury cars.

Method used

A method involving the application of a solvent-based clear paint composition onto a base material, followed by a cover material, and an aging treatment to cure the laminate, utilizing a cover material that captures and passes solvents, ensuring a clear layer with predetermined characteristics.

Benefits of technology

This method significantly reduces VOC emissions, achieves a clear layer with consistent quality, excellent weather and scratch resistance, and enhances surface smoothness, while maintaining aesthetic appeal, all within a shorter time frame.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567046000016
    Figure 0007567046000016
  • Figure 0007567046000017
    Figure 0007567046000017
  • Figure 0007567046000001
    Figure 0007567046000001
Patent Text Reader

Abstract

[Abstract] [Problem] To provide a method for manufacturing a layered body, a layered body that is obtained via said method, and a molding method and a molded body in which said layered body is used, said method for manufacturing a layered body being convenient, minimizing environmental burden such as due to the release of carbon dioxide and VOCs, and being able to provide a clear layer of a consistent quality. [Solution] Obtained are a method for manufacturing a layered body, a layered body, and a molding method and a molded body in which said layered body is used, said method for manufacturing a layered body being characterized by including various steps in which a solvent-type clear coating composition is applied on a base material, a covering material is positioned on the solvent-type clear coating composition while the solvent-type clear coating composition is in an uncured state, and an uncured layered body that is thus obtained and is formed from the base material, the solvent-type clear coating composition, and the covering material is subjected to an aging process, thereby curing the uncured solvent-type clear coating composition and forming a cured layered body that includes a cured clear layer, wherein the covering material is a material that is capable of trapping, transmitting, or both trapping and transmitting a solvent in the solvent-type clear coating composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a laminate having a clear layer, a laminate obtained thereby, a method for producing a composite coating film, a composite coating film obtained thereby, a method for producing an insert molded body using the same, and a molded body, and a clear layer obtained from the above laminate. [Background technology]

[0002] Metal substrates constituting the bodies of automobiles and the like are generally covered with a coating film having a laminated structure consisting of an undercoat layer for rust prevention and to ensure adhesion to the upper layer, an undercoat layer and a topcoat layer for reinforcement and coloring, and a clear layer for coating surface protection and decoration.

[0003] Each layer of such a laminate, particularly the intermediate coat layer, top coat layer, and the outermost clear layer, can be produced by a conventional coating technique of spraying a fluid paint, etc. Alternatively, it is at least theoretically possible to apply the paint by forming and curing the paint in advance to obtain a flexible film, which is then adhered to the lower layer (intermediate coat layer or top coat layer), and one example of this is a decorative film applied to an existing coating film.

[0004] Among the above, in the case of painting by so-called coating using a fluid paint, the desired material can be selected, and a coating film that is flawless in terms of aesthetics and physical properties can be obtained, but the time from coating to hardening is long, and during that time, it is necessary to observe the hardening of the coating film on the surface of the product or part (substrate) such as an automobile under constant aging and clean conditions. Furthermore, in painting by spray application, etc., there are concerns that most of the paint is released into the atmosphere without adhering to the object to be coated, and that the impact of CO2 and organic solvents (VOCs) generated during coating may have on the environment.

[0005] On the other hand, in the method of forming a coating film by extrusion molding or the like and applying it to the object to be coated, the material used must be suitable for extrusion molding, but considering the heating conditions of extrusion molding, there are limitations on the types of resins that can be used for film formation. In addition, the decorative film or clear layer obtained by such a method must meet the physical property requirements, such as weather resistance, chemical resistance, and scratch resistance (e.g., resistance to scratches caused by car washes), when exposed to wind, rain, and high temperatures. With only a limited number of materials that meet the conditions required at the molding stage, a film that satisfies all of the above physical properties has not yet been reported.

[0006] Furthermore, depending on the application of the film, it is desirable to produce a clear layer that satisfies the aesthetics required for private cars, including luxury cars. In order to mass-produce flexible films on an industrial scale, they are generally wound up and stored, and a predetermined winding speed is required to improve productivity, but high-speed transport puts a load on the surface of the film, making it difficult to produce a clear layer that satisfies the aesthetics required for private cars, including luxury cars. In addition, as long as the winding speed is maintained at a predetermined level, it is not easy to improve the condition of the film surface by performing some additional treatment on the film surface after molding and before winding. Summary of the Invention [Problem to be solved by the invention]

[0007] In view of the above-mentioned conventional techniques, the present invention aims to provide a method for producing a laminate which is easy and reduces the burden on the environment and can provide a clear layer of consistent quality, as an alternative to the production of coating films obtained by conventional painting (coating), and a laminate obtained by this production method.

[0008] A further object of the present invention is to provide a method for producing a composite coating film from the above-mentioned laminate, a composite coating film obtained thereby, a method for producing a molded article using the composite coating film and a molded article, and a clear layer obtained from the above-mentioned laminate. [Means for solving the problem]

[0009] As a result of intensive research, the present inventors have found that the above-mentioned problems can be solved by A solvent-based clear coating composition is applied onto a base material; A cover material is placed on the solvent-based clear coating composition while the solvent-based clear coating composition is in an uncured state; The method includes the steps of subjecting the uncured laminate composed of the base material, the solvent-based clear coating composition, and the cover material obtained in this way to an aging treatment to cure the uncured solvent-based clear coating composition and form a cured laminate containing a cured clear layer, It has been found that this can be achieved by a method for producing a laminate, in which the cover material is a material capable of trapping, passing through, or both trapping and passing through, the solvent in the solvent-borne clear coating composition.

[0010] In the above manufacturing method, the cover material has a density of 0.09 to 1.4 g / cm 3 It is preferable that the support member 100 is made of a resin having a water absorption rate of 0.3 to 7.0%, a surface roughness of Ra 1 μm or less, and a pencil hardness of 6B to 4H.

[0011] In the above-mentioned manufacturing method, a solvent-based primer coating composition is applied in advance onto a base material, A solvent-based clear coating composition is applied onto the solvent-based primer coating composition; A cover material is placed on the solvent-based clear coating composition while the solvent-based clear coating composition is in an uncured state; It is also possible to subject the thus obtained uncured laminate consisting of the base material, the solvent-based primer coating composition, the solvent-based clear coating composition and the cover material to an aging treatment.

[0012] Furthermore, the above-mentioned manufacturing method may further include a step of winding the uncured laminate into a roll, and the roll may also be subjected to an aging treatment.

[0013] In the above manufacturing method, the cover material may be cellulose, acetylated cellulose, (meth)acrylic resin, polyamide, porous polypropylene and porous polyethylene, or a polyolefin nonwoven fabric.

[0014] In the above manufacturing method, the solvent-borne clear coating composition may be a composition containing one or more types of hydroxyl group-containing (meth)acrylic resin and an isocyanate crosslinking agent, or a composition containing a urethane polymer solution, and may further contain a weather resistance stabilizer.

[0015] A cured product of a polypropylene composition containing a polypropylene selected from a homopolymer, a random copolymer, or a block copolymer of polypropylene, or a composition containing an acrylonitrile, butadiene, and styrene copolymer can be used. Both the polypropylene composition and the composition containing an acrylonitrile-butadiene-styrene copolymer preferably contain a hindered amine-based weather resistance stabilizer.

[0016] In the above-mentioned manufacturing method, the base material may be a cured product of a composition containing a propylene homopolymer, random copolymer or block copolymer, or an acrylonitrile-butadiene-styrene copolymer, and it is preferable that the base material contains a hindered amine-based weather resistance stabilizer.

[0017] The base material has a density of 0.09 to 1.4 g / cm 3 The base material may be made of a resin having a water absorption rate of 0.3 to 7.0%, a surface roughness of Ra 1 μm or less, and a pencil hardness of 6B to 4H. The base material may be cellulose, acetylated cellulose, (meth)acrylic resin, polyamide, porous polypropylene, porous polyethylene, or a polyolefin nonwoven fabric.

[0018] The object of the present invention is also achieved by a laminate comprising a base material, a cured clear layer, and a cover material, which is obtained by any one of the above-mentioned production methods.

[0019] Another object of the present invention is to provide a method for producing a composite coating film, which is characterized in that a composite coating film containing a base material and a cured clear layer is produced by removing a cover material from the above-mentioned laminate. This is achieved by:

[0020] Furthermore, the object of the present invention is achieved by a composite coating film obtained by the above-mentioned production method.

[0021] The above object of the present invention can be achieved by a method for producing a molded article, which comprises applying the above-mentioned composite coating film to a substrate to produce a molded article having a clear layer, The molded article is formed by insert molding the composite coating film onto a substrate, and can have the clear layer as the outermost coating.

[0022] The substrate may be selected from automobiles, motorcycles, bicycles, road materials, ships, rail vehicles, aircraft, buildings, building materials, furniture, household appliances, containers, musical instruments, stationery, sporting goods, toys, parts or portions thereof.

[0023] The above object of the present invention is also achieved by a molded article obtained by the above production method.

[0024] The object of the present invention is also achieved by a laminate comprising a base material, a cured clear layer, and a cover material, which is obtained by the above-mentioned manufacturing method.

[0025] Furthermore, the object of the present invention is also achieved by a clear layer obtained by removing the base material and the cover material from the above laminate. Effect of the Invention

[0026] According to the method for producing a laminate of the present invention, the solvent in the solvent-based clear coating composition is effectively removed by directly applying a cover material having a predetermined property to the solvent-based clear coating composition. That is, the cover material plays a role of capturing, passing, or capturing and passing the solvent. As a result, the production method of the present invention significantly reduces the burden on the environment compared to conventional coating (fluid coating) in which spray coating is performed directly on the coating object, and provides a method for producing a laminate including a clear layer of constant quality (i.e., no variation in quality depending on the type of clear coating composition) with fewer production steps, simply and in a short time. Furthermore, the production method of the present invention can provide a laminate including the above-mentioned clear layer, or such a clear layer and an optional primer layer, and a base layer. Furthermore, the cover material contained in the obtained laminate can be peeled off, and the laminate can be attached to a substrate (coating object) such as an automobile body or a part (part) thereof by insert molding or the like so that the clear layer becomes the outermost layer coating, thereby obtaining a molded product such as an insert molded product coated with a clear layer having the above-mentioned properties.

[0027] According to the manufacturing method of the present invention, it is possible to obtain a coating film having excellent quality at least equivalent to that of a coating in terms of physical properties such as weather resistance, chemical resistance, scratch resistance, etc., depending on the type of clear coating composition. Furthermore, in a specific embodiment, it is possible to obtain a high-quality clear layer, a laminate containing the same, and a composite coating film that provide improved surface smoothness and excellent aesthetics. [Brief description of the drawings]

[0028] [Figure 1] FIG. 1 is a diagram illustrating a method for producing a laminate according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view illustrating a method for producing a laminate and a molded article using the same according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] In the manufacturing method of the present invention, a laminate including a clear layer is manufactured, which can be used for surface coating of a coating target (also called a substrate). There is no particular limitation on the substrate to which the laminate of the present invention is applied, but it is mainly applied to substrates made of synthetic resin, especially thermoplastic resin. Representative examples of substrates include synthetic resins in general, including resins that have been developed in recent years that are lightweight yet have excellent strength, and in particular, materials that can be applied to vehicles and bodies, including automobiles, motorcycles, etc., and their parts and components.

[0030] In the present invention, a composite coating film obtained by peeling off the cover material from a laminate formed by laminating the base material (base film) of the present invention, a primer layer (primer film) as an optional configuration, a clear layer (clear film), and a cover material (cover film) can be applied to a coating object made of such a synthetic resin by composite molding such as insert molding. It is preferable that the cover material is maintained as a part of the laminate for protecting the clear layer until it is applied to the coating object, and is peeled off immediately before application to the coating object.

[0031] When the composite coating film is applied to insert molding, (i) the composite coating film is introduced into a mold for insert molding so that the base film side is in contact with the object to be coated (solid workpiece), or (ii) the composite coating film is arranged so that the clear layer side faces the inner surface of the mold, and the resin is injection molded, so that the composite coating film is deformed into the shape of the mold by the pressure and heat of the resin in the heated and molten state. As a result, in the case of (i) above, both the material of the base film and the surface of the synthetic resin workpiece, which is the material to be coated, are melted and fused / thermally fused, and the two are firmly integrated. In addition, in the case of (ii) above, the molten resin is fused / thermally fused with the surface of the melted and deformed composite coating film, and firmly integrated. Furthermore, when a colored base film or an ink layer additionally printed on the base film is used, the clear layer protects it, and a multi-functional layer consisting of multiple layers is laminated on the object to be coated at once.

[0032] The order of lamination of the base material, primer layer and clear layer is as described above, but as long as it does not adversely affect the performance, quality or manufacturing process of each layer constituting the laminate, it is possible to provide another layer, for example a printed layer, between each base material and primer layer, and between the primer layer and the clear layer. Similarly, the composite coating film can be applied to the object to be coated after necessary pretreatment.

[0033] The method for producing the laminate of the present invention will be described below.

[0034] In the present invention, when indicating the positional relationship of each composition or layer, the term "on" in expressions such as "on a base material" does not necessarily mean that the lower layer and the upper layer are provided in contact with each other, but includes the case where these layers are present separately below and above, that is, where another layer is interposed between the two phases. In contrast, the expressions "directly on" or "directly" mean that the upper and lower layers are provided in contact with each other, so far as the positional relationship is indicated.

[0035] The laminate of the present invention includes a step of applying a solvent-based clear coating composition (also referred to as a clear composition) onto a base member (clear composition application step), A step of placing a cover member on the solvent-based clear coating composition while the solvent-based clear coating composition is in an uncured state (cover member placement step); and The product is manufactured through various steps, including a step of subjecting the uncured laminate of the solvent-based clear coating composition, which is composed of the base material obtained in this manner, the solvent-based clear coating composition, and the cover material, to an aging treatment to harden the solvent-based clear coating composition to form a clear layer (aging hardening step).

[0036] Furthermore, prior to the above-mentioned clear composition application step, a step of applying a solvent-based primer coating composition onto the base material (primer composition application step) can also be carried out.

[0037] In this case, generally, a solvent-based primer coating composition (also called a primer composition) is applied in a relatively thin film thickness (e.g., 5 μm), and after application, curing can be performed only by a drying process at a high temperature (e.g., 140° C.) before applying the clear composition. The cured primer layer can be optionally pretreated, and then the clear composition can be applied. Note that the term "solvent-based" in the solvent-based primer coating composition and the solvent-based clear coating composition of the present invention means that each composition contains an organic solvent, which will be described later.

[0038] After application of the clear composition, the above-mentioned cover material arrangement process is carried out, and the laminate consisting of the obtained base material, an optional primer layer, the solvent-based clear coating composition, and the cover material is subjected to an aging treatment, and the solvent-based clear coating composition is hardened to form a clear layer (aging hardening process).

[0039] In the present invention, the above-mentioned specified cover material is placed on the uncured solvent-based clear coating composition so that the solvent to be removed from the clear composition before curing is effectively removed. The solvent to be removed is the residual solvent used in the production of the primer composition and the clear composition or the organic solvent that may be added later, particularly volatile organic solvents (VOCs). Here, volatile organic solvents (VOCs) are defined as "organic compounds that are gaseous when discharged or dispersed into the atmosphere" in Article 2, paragraph 4 of the Air Pollution Control Act, and are about 200 types of compounds. In the present invention, in order to minimize the emission of such VOCs, they are captured by the cover material, or they can be captured after passing through the cover material, thereby minimizing air pollution. In addition, the method of the present invention is particularly useful in that it is possible to produce a laminate, composite layer, or clear layer including a clear layer that has an appearance and physical properties equal to or better than those of coating by spray spraying, without using a method such as spray spraying in which organic solvent diffusion is unavoidable.

[0040] In the present invention, volatile organic solvents (VOCs) contained in the clear composition, such as cyclohexane, toluene, xylene, ethylbenzene, n-butyl acetate, isobutyl acetate, acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, isophorone, ethyl acetate, tetrahydrofuran, 1,4-dioxane, acetonitrile, N,N-dimethylformamide, and the like, particularly n-butyl acetate and xylene, are efficiently captured in the cover material, or can be captured even after passing through it, or can be easily produced as desired laminates, composite layers, and clear layers while minimizing the emission of organic solvents without using a spraying means.

[0041] Details of each of the above steps are as follows.

[0042] [Primer composition application process] In the present invention, first, a primer composition is applied to a base material.

[0043] The primer composition is a material that imparts a predetermined adhesive strength to the coating film and forms a primer layer. Any known material can be used as the primer composition, and there is no particular restriction, but as the main component, acrylic, ethylene vinyl acetate, urethane, epoxy resins, modified polypropylene resins, and mixtures thereof are used.

[0044] The types of base materials will be described later, but for example, when the base material is mainly made of acrylonitrile-butadiene-styrene copolymer (ABS resin), it is common to omit the application of a primer. However, when it is necessary to prevent the penetration of solvents into the ABS resin, a protective film or undercoat film is required.

[0045] The coating thickness of the primer composition is, for example, 1 to 100 μm, preferably 3 to 65 μm, and particularly 3 to 10 μm. If it is 1 μm or more, the coating of the primer composition can be stable and uniform, and if it is 100 μm or less, the flexibility required when the film is wound up can be ensured.

[0046] The solid content (25°C) of the primer composition is generally 5 to 50 mass%, preferably 10 to 30 mass%, and the viscosity (25°C) is generally 10 to 50 mPa.s, preferably 20 to 30 mPa.s. The solid content and viscosity are appropriately adjusted according to the coating method of the primer composition, but by making them 10 mPa·s or more, the spreadability during coating of the composition is ensured, and by making them below, the film thickness of the cured product is sufficient. After coating, the primer composition is preferably placed in a drying oven at 40 to 200°C, preferably 70 to 150°C, for 3 to 30 minutes, and dried for, for example, 30 minutes until the solid content of the primer composition becomes about 100%. When manufacturing a laminate or composite coating film that does not include a primer layer, it goes without saying that this step is omitted.

[0047] [Clear composition application (coating) process] When a laminate or composite coating containing a primer layer is produced, a clear composition is applied to the primer layer on a solid base material. On the other hand, when a laminate or composite coating not containing a primer layer is produced, a clear composition is applied to a substrate. The clear composition is generally a material that forms a clear coat layer as the outermost layer of a coating, and can impart a transparent feel to the color of the colored base material to impart an aesthetic appearance. Furthermore, the clear layer itself can maintain a transparent aesthetic and have physical properties including weather resistance, chemical resistance, and scratch resistance.

[0048] In the present invention, the term "composition" refers to a composition in an uncured state, and the terms "layer" such as a primer layer and a clear (coat) layer refer to cured layers.

[0049] The coating thickness of the clear composition is, for example, 10 to 150 μm, preferably 10 to 100 μm, and particularly 20 to 50 μm. If it is 10 μm or more, the coating of the clear composition can be stable and uniform, and if it is 150 μm or less, the flexibility required for winding the film can be ensured.

[0050] The solid content (25°C) of the clear composition is generally 20-90% by mass, preferably 30-60% by mass, and the viscosity (25°C) is generally 10-100 mPa·s, preferably 20-70 mPa·s. The solid content and viscosity are appropriately adjusted according to the coating method of the clear composition, but by making the solid content 20% by mass or more and / or the viscosity 10 mPa·s or more, the spreadability during coating of the composition is ensured, and by making the solid content 90% by mass or less and / or the viscosity 100 mPa·s or less, the film thickness of the cured product is sufficient. In addition, after coating, the clear composition is preferably dried at 50-200°C, preferably 50-150°C, for example, for 30 minutes until the solid content of the clear composition becomes 98%, preferably about 100%.

[0051] The viscosity of each of the primer and clear compositions was measured using a TVB-10M viscometer (manufactured by Toki Sangyo Co., Ltd.) and the values ​​shown are given below.

[0052] The primer composition and the clear composition are preferably applied by coating using a commonly used coating machine such as a roll coater, a flow coater, or a dipping type coating machine, or by coating using a brush, a bar coater, an applicator, etc. Considering the continuous carrying out of the pre- and post-treatment steps and the accurate control of the coating amount, a roll coater is preferably used. This coating method allows the base material to be coated with a necessary and sufficient amount of coating quickly and with a constant film thickness.

[0053] As another application method, spray application can be selected. In that case, in light of the object of the present invention, it is desirable to take sufficient consideration of the environment, use the minimum amount of clear composition necessary to obtain a clear layer, and take measures to suppress emission outside the base material, as in the above-mentioned preferred method.

[0054] [Cover material application process] After the above drying treatment, an uncured laminate is obtained by laminating a solid cover material such as a film on the uncured clear composition, i.e., on the side of the clear composition opposite the above base material (and primer layer).

[0055] The cover material is placed on the uncured clear composition immediately after application of the clear composition, preferably within 1 to 5 minutes after application, so as to cover the entire surface of the uncured clear composition without disturbing the surface. A commonly used laminating device, such as a laminator, can be used.

[0056] The above process provides an uncured laminate including the base material of the present invention, an optionally cured primer layer, an uncured clear composition, and a cover material. The laminate thus obtained is subjected to aging treatment at a temperature above room temperature (25°C) and below the curing temperature of each composition, preferably 25 to 80°C, particularly preferably 40 to 70°C, and particularly preferably 40 to 60°C, usually for 1 to 7 days, to cure the clear composition and the uncured primer composition, if any, to provide a cured laminate having a clear layer and, if necessary, a primer layer.

[0057] The organic solvent or gas contained in the clear composition captures, passes through, or captures and passes through the solvent in the solvent-based clear coating composition. Here, "capture" includes the organic solvent or gas contained in the clear composition arranged in contact with the cover material, and the liquid or gas generated by the reaction of the components in the clear composition being taken into the material, penetrating or adsorbing into the structure of the cover material, or adhering to the surface of the cover material or the wall surface of the pores in the case of a porous material, and "passing through" means that the above organic solvent, liquid, or gas passes through the inside of the cover material, regardless of the presence or absence of the above capture, and is brought to the outside of the surface of the cover material that is not in contact with the clear composition / clear layer.

[0058] In the present invention, the clear composition is present between the base material and the cover material, and is fixed between them, so that the organic solvent is captured by the cover material due to the surface tension unique to the clear composition and the capillary phenomenon of the cover material, and most of it eventually passes through the cover material. Highly volatile organic solvents pass through the cover material without necessarily being captured by it. That is, gas (air, etc.) present in the organic solvent or gas (CO2, etc.) or liquid generated during the curing reaction also passes through the cover material during the aging treatment, and the bubbles generated at this time are also broken.

[0059] Furthermore, the clear composition, particularly the surface of the clear composition, is affected by the covering material that is provided directly on it.

[0060] In the present invention, the cover material has a density of 0.09 to 1.4 g / cm 3 , preferably 1.2 to 1.4 g / cm 3 By having all of the physical properties of water absorption of 0.3 to 7.0%, preferably 0.5 to 6.5%, surface roughness Ra of 1 μm or less, preferably 0.01 μm to 1 μm, more preferably 0.01 μm to 0.1 μm, and surface pencil hardness of 6B to 4H, preferably 2B to 4H, and particularly preferably 2H to 4H, the volatilization of the solvent remaining in the uncured clear composition is promoted, and the aesthetic appearance and physical properties of the surface of the clear layer of the obtained laminate are improved. By using a cover material having the above properties, the smoothness of the cover material is transferred to the clear layer, forming a clear layer that is smooth, rich in smoothness, and in some cases, excellent in gloss. Furthermore, by taking into consideration the properties such as physical properties required for the desired clear layer, the clear composition is selected, and the range of each of the above properties of the cover material is also set to be appropriate according to the type of clear composition, the physical properties of the clear composition are maximized, and the smoothness of the cover material surface is transferred to the clear layer. For this transfer, it is necessary to have a hardness appropriate for the clear composition. Examples of suitable combinations of the clear composition and the cover material will be described later.

[0061] In addition, the laminate of the present invention, which includes a base material, a clear layer, and a cover material, can be applied to a composite coating film on a coating object in a state in which the cover material is peeled off from the laminate. In other words, the cover material is peeled off after the clear layer is cured, so a certain degree of peelability is also required.

[0062] When using a clear layer for the exterior of an automobile or the like, it is conceivable to use a covering material with a small surface roughness. However, when manufacturing a clear layer with a texture reminiscent of fibrous materials, such as for the interior of an automobile or building, it is also possible to intentionally increase the surface roughness Ra.

[0063] The above values ​​were determined according to the following methods / standards, and in this specification, each value conforms to these unless otherwise specified.

[0064] The density was measured in accordance with JIS K7112:1999, Plastics - Non-foamed plastics - Measurement method for density and specific gravity.

[0065] The water absorption rate is measured according to JIS K7209:2000 - Determination of water absorption rate of plastics when the thickness of the sample is 100 μm or more, and according to JIS K7129:2008 - Determination of water vapor transmission rate when the thickness of the sample is less than 100 μm (both are water absorption rate and water vapor transmission rate when the cover material sample is in contact with the clear composition surface for 24 hours). Note that, although the above JIS refers to "water absorption rate", in the present invention, this is read as organic solvent absorption rate, and the value is obtained by the same test.

[0066] The surface roughness Ra was measured in accordance with the arithmetic roughness Ra of JIS B 0601:1994 and JIS B 0031:1994.

[0067] The surface pencil hardness was measured in accordance with JIS K 5600-5-4 "General test methods for paints - Part 5: Mechanical properties of coatings - Section 4: Scratch hardness (pencil method)".

[0068] The above-mentioned characteristic values ​​of the cover material can be appropriately selected according to the clear composition immediately below it, for example, as follows. That is, (1) Density 1.2~1.4g / cm 3 A cover material (specific example: TAC film) with a water absorption rate of 3.0 to 7.0%, a surface roughness of Ra 0.01 μm to 0.1 μm, and a surface pencil hardness of 2H to 4H is used for clear compositions containing poly(meth)acrylate and aminoplast components such as melamine as resin components, clear compositions containing poly(meth)acrylate and poly(blocked)isocyanate as resin components, and acrylic-urethane resins (for example, a clear layer containing urethane-modified (meth)acrylate as the main component can be obtained).

[0069] (2) Density 1.1~1.2g / cm 3 A cover material (specific example: acrylic film (poly(meth)acrylate) having a water absorption rate of 0.3 to 0.5%, a surface roughness of Ra 0.1 μm to 1 μm, and a surface pencil hardness of 6B to 2H is used for clear compositions containing (mer)acrylate as a resin component. Due to the characteristics of the material, unmodified (mer)acrylate itself has poor physical properties such as chemical resistance and scratch resistance when compared with the modified (mer)acrylate in (1) above. However, according to the production method of the present invention, a hardened layer having physical properties equal to or greater than those obtained by conventional coating of unmodified (mer)acrylate and having improved surface smoothness and gloss can be obtained, making it effective, and particularly used in fields such as automotive interior materials, interior panels for buildings, and decorative items.

[0070] (3) Density 0.09~1.0g / cm 3Cover materials (specific examples: porous polypropylene film, porous polyethylene film, polyolefin nonwoven fabric) with a water absorption rate of <0.01%, a surface roughness of Ra 0.1-1 μm, and a surface pencil hardness of 6B-H can, in some cases, be subjected to a pretreatment such as a corona treatment on the surface, and used for clear compositions containing resin components such as poly(meth)acrylate and poly(blocked)isocyanate as the resin components, and clear compositions containing resin components such as a clear layer mainly composed of an acrylic-urethane resin, for example, a urethane-modified (meth)acrylate.

[0071] (4) Density 1.1~1.2g / cm 3 , water absorption rate 1-2%, surface roughness Ra 0.1-1 μm, surface pencil hardness B-H (specific example: polyamide film) is used for a clear composition containing poly(meth)acrylate and aminoplast components such as melamine as resin components. Polyamide has low physical properties such as scratch resistance compared to the modified (meth)acrylate case in (1) above due to the characteristics of the material, but according to the manufacturing method of the present invention, a layer having physical properties equal to or greater than those of a coating film by conventional coating with polyamide and having improved surface smoothness and gloss can be obtained, so that it is suitable for use as a coating film for building material parts, home appliances, etc.

[0072] As described above, by using a suitable cover material in accordance with the properties of the clear composition, it is possible to achieve excellent surface properties (gloss, smoothness) that exceed those of a painted coating, and sufficient physical properties for each material, in accordance with the characteristics of each material.

[0073] Specific examples of materials constituting the cover material include cellulose, acetyl(ated)cellulose such as monoacetyl cellulose, diacetyl cellulose, and triacetyl cellulose (TAC), (meth)acrylic resin or polyamide, acrylic resin, cycloolefin, porous polyester film, porous polyolefin film, and nonwoven fabrics thereof, among which, preferred are cellulose, acetylated cellulose such as monoacetyl cellulose, diacetyl cellulose, and triacetyl cellulose (TAC), polyamide, (meth)acrylic resin, porous polypropylene and porous polyethylene, or polyolefin nonwoven fabrics, and particularly preferred are acetylated cellulose and polyamide. These may be used alone or as a mixture of multiple types, and are selected according to the properties of the clear composition that the cover material covers.

[0074] Of the above materials, it is particularly preferable to use triacetyl cellulose alone as a material that can clamp the uncured clear composition between the cover material and the base material, that allows volatile substances such as the organic solvent of the clear composition and air to pass through during aging, that transfers the smoothness of the cover material to the clear layer surface, and that is easily peeled off after the clear layer is cured.

[0075] In the present invention, it is preferable that the cover material does not contain additives. If the cover material contains additives, when the clear composition in contact with it hardens, the organic solvent of the clear composition will pass through and move through the cover material while incorporating the additives of the cover material, and the additives may bleed into the clear composition / clear layer and stain the clear layer surface. If the cover material does not contain additives, this possibility is eliminated, leading to the assurance of excellent surface quality of the clear layer. Furthermore, it also reduces the cost and effort of production. Among the above examples of cover materials, particularly cellulose, acetylated cellulose such as monoacetyl cellulose, diacetyl cellulose, and triacetyl cellulose (TAC), and acrylic resins can form a plane with excellent smoothness without using additives.

[0076] The cover material is generally produced as a film, and the thickness is in the range of 10 to 100 μm, preferably 25 to 80 μm, and particularly preferably 40 to 80 μm. By making the thickness 10 μm or more, it can adhere to the surface of the clear resin coating composition coated therewith and provide smoothness, and by making it 100 μm or less, the solvent in the clear composition can be well adsorbed and released. In addition, the film-like cover material (hereinafter also referred to as the cover film) is generally made into a roll (roll) in consideration of its storage and the convenience of unwinding when bringing it onto the clear composition, and so on, and if the thickness is within the above range, winding and unwinding can be performed well.

[0077] The aging treatment of the above-mentioned clear composition can be carried out using equipment such as a heating dryer, a thermostatic drying chamber, etc. By controlling the temperature at a constant temperature, the coating film hardens at a constant speed, the reaction state of the composition becomes stable, and uniform hardening is achieved deep into the coating film.

[0078] Furthermore, in order to produce a film-like covering material, known film forming methods such as melt extrusion molding, solution casting, coextrusion, calendaring, lamination, etc. are used. When used to obtain a clear layer with high surface smoothness, it is important that a cover film with excellent surface smoothness can be produced regardless of which of the above film forming methods is used for the covering material. This is because the smooth surface of the covering material is adhered to the surface of the uncured clear composition, and the smoothness is transferred to the clear layer. In addition, since the covering film is generally made into a roll after extrusion, it is also produced using known equipment that combines film forming and winding.

[0079] The uncured laminate obtained as described above can be produced sequentially by a conveying system, and the uncured laminate is generally aged in a wound state and stored and shipped as is. Fig. 1 is a schematic explanatory diagram of a winding process that can be applied to the laminate manufacturing method of the present invention. An example of a winding method for an uncured laminate will be described with reference to the same figure.

[0080] In the roll laminating device 1 in Fig. 1, a roll-shaped base material (base film) 10 is held by a roller 10a, and the unwound base material 10 is transported in the direction of the arrow a. A clear composition 14 is uniformly coated on the upper surface of the base material 10 by a roll coater device 12, and the base material 10 is transported in the direction of a drying oven 16.

[0081] The clear composition 14 applied onto the base material 10 is dried by passing through the drying oven 16. Although FIG. 1 illustrates a case where a clear layer is directly provided on the base material, when a primer layer is provided on the base material, a roll coater device (not shown) and a drying oven (not shown) can be further used to apply and dry the primer composition to the base material after unwinding in FIG. 1, and then the above-mentioned clear composition 14 can be applied thereto. Alternatively, a laminate (hereinafter referred to as a dry film) having a primer layer in which a primer composition has been applied and dried by passing it once through a roll laminator device can be used as the base material.

[0082] On the other hand, a roll-shaped cover material 18 (or a dry film having a primer layer) is supported by a roller 18a, unwound in the direction of arrow b, and brought onto the clear composition 14 on the base material 10 (or a dry film having a primer layer), thereby being laminated in a laminating section 20. The laminating section 20 laminates the base material 10 (or a dry film having a primer layer), the clear composition 14, and the cover material 18 between a first laminating roll 20a and a second laminating roll 20b. The laminate (laminate with uncured clear composition) 22 obtained by lamination is continuously conveyed in the directions of arrows c and d, and is wound up by a roller 22a, which is a means for winding up the laminate 22. A roller 24 is used as a tensioning means to give a predetermined tension to each film and the laminate.

[0083] The lamination of the cover material is performed at a lamination pressure of 0 to 7 kg / cm by adjusting the pressure of the first lamination roll 20a and the second lamination roll 20b. 2 , preferably 1 to 6 kg / cm 2 and the temperature can be adjusted to 15 to 35° C., preferably 20 to 25° C. When using a winding device such as that shown in FIG. 1, these values ​​can also be monitored by a control system (not shown).

[0084] When the laminate of the present invention is produced as a roll, the winding speed does not particularly affect the quality of the clear layer, but from the viewpoint of productivity, the conveying speed / lamination speed can be usually 10 to 50 m / min, preferably 10 to 20 m / min.

[0085] In addition, when the laminate film is wound up, the surface of the cover material and the back surface of the base material come into contact, so depending on the type of base material, the roughness or texture of the back surface may affect the surface smoothness of the cover material surface or the clear layer. In order to improve the surface smoothness of the clear layer, particularly when the winding pressure is relatively large depending on the device used, it is preferable to provide a protective layer (protective film) on the back surface of the base material. Alternatively, it is possible to use a base material with mirror surfaces on both sides, or two base materials with one mirror surface and the other textured surface, and to use a two-layered base material with both outer surfaces mirrored by bonding the textured surfaces of the two base materials together so that they face each other. However, since it is expected that the provision of a protective layer will increase costs, it is also important to set the winding pressure according to the characteristics of the clear composition so that the surface smoothness of the clear layer is not impaired even without the provision of a protective layer.

[0086] In addition, by using the same material as the cover material for the base material, it is possible to prevent the condition of the back surface of the rolled base material from affecting the surface of the clear layer.

[0087] The laminate of the present invention is not limited to the above-mentioned method of manufacturing the laminate as a roll. For example, the laminate of the present invention can be obtained by preparing a base material of a certain size and shape, such as a long or rectangular shape, applying a clear composition to the base material, and placing a cover material on the upper surface of the clear composition to adhere the clear composition and the cover material to each other. In this case, too, a smooth or glossy clear layer can be formed after peeling off the cover material by selecting the clear composition and the type of cover material. In addition, even when stacking laminates of a predetermined shape and storing them, it is also possible to increase the thickness of the cover material or provide the above-mentioned protective layer on the surface so that the roughness or texture of the back surface of the base material (for example, the texture of a polypropylene base film) is not transferred to the cover material or clear layer.

[0088] In this case, the protective layer must not impair the above-mentioned effects of the cover material, and therefore a layer having similar properties to the cover material, particularly an acetylated cellulose film, a polyester film, a polypropylene film, a polyethylene film, a polyolefin nonwoven fabric, etc., can be used.

[0089] In either case, it is preferable that the clear layer and the cover material are manufactured with uniform thickness on the base material, but the end faces of the laminate may have some unevenness because the clear layer may protrude beyond the base material and / or the cover material, or may not be applied to the entire surface of the base material and / or the cover material may be recessed inside them, etc. In this case, the end faces can be cut as necessary to manufacture a laminate without unevenness on the end faces, for example, a roll-shaped laminate.

[0090] [Aging hardening process] The laminate in the form of a roll or other shape obtained as described above is subjected to an aging treatment. In the aging treatment, the laminate consisting of the base material, the clear composition, and the cover material is kept as it is at a temperature of, for example, room temperature to 80°C and atmospheric pressure for about 1 day (24 hours) to 7 days to cause the reactive compound in the clear composition to react. This results in a cured product of the clear composition, i.e., a clear layer.

[0091] The cured clear layer is generally transparent or translucent, preferably transparent, and has a particularly high light transmittance of 90% or more, and can form a surface with excellent gloss of 90 or more, preferably 92 or more, measured using a Cat. No. 4442 Micro Gloss 20° (also called gloss 20°) surface gloss meter (manufactured by Tetsutani Co., Ltd.).

[0092] [Manufacturing of composite coating film] The composite coating film can be obtained by peeling off the cover material from the laminate in which each layer has been cured (cover material peeling step). Peeling can be easily done by hand, but can also be done with a film peeling device (e.g., a protective film peeling device).

[0093] After peeling off the cover material, if a primer composition is applied, a composite coating film having a base film / primer layer / clear layer in that order is obtained, and if a clear layer is applied directly onto the base film, a composite coating film of base film / clear layer is obtained; in either case, a film-like composite coating film can be obtained.

[0094] If desired, other layers may be provided between the base film and the primer layer, and between the primer layer and the clear layer. For the application of other layers, see, for example, JP-A-2000-301844, JP-A-1992-366632, JP-A-1992366633, JP-A-2010-234366, and JP-A-2011-093306.

[0095] [Application of laminates and composite coatings] 2 is a diagram for explaining the laminate of the present invention and the method for producing a molded article using the same, and is a cross-sectional view showing a laminate (cured laminate) 100 in which the clear layer has been cured by the above-mentioned aging treatment, applied to a substrate 200. The laminate 100 has a primer layer 130, a clear layer 140, and a cover material 150, which are arranged in this order on a base film 120. Note that the laminate 100 may be provided with a protective film (not shown) during storage or aging, as described above.

[0096] Here, as a specific example, the manufacture of an insert molded body will be described. In application to an aircraft 200, the laminate 100 is arranged so that the base film 120 side is in contact with the surface of the substrate 200, for example, a work (semi-processed product) such as an automobile body, a part, or a part thereof (preferably made of synthetic resin), and if a protective film is present, it is peeled off, and the cover material 150 is peeled off, and the composite coating film (a laminate of the base film 120, the primer layer 130, and the clear layer 140) is introduced into a mold (not shown) for insert molding. Thereafter, by injecting synthetic resin into the mold from the inside of the work, the base film 120 of the composite coating film melts due to the heat of the molten synthetic resin and fuses with the substrate 200, and preferably the surface portion of the synthetic resin to be coated melts and fuses with the molten base film, and is integrated through subsequent cooling. That is, the substrate is thereby coated with the composite coating film to form an insert molded body. As mentioned above, the primer layer is provided optionally, and regardless of the presence or absence of the primer layer, the clear layer constitutes the outermost coating layer of the insert molding.

[0097] [Single clear layer] By preparing the base material in a peelable state, it is possible to peel not only the cover material but also the base material from the laminate, and produce a single clear layer (clear sheet or film). This single layer is used in various forms such as a colorless transparent or colored transparent cured clear sheet or film, a block, or an indefinite shape, as exterior parts of automobiles, building materials such as fittings, windows, and partitions, office products, daily necessities, stationery, toys, decorative items, or the outermost exterior parts, parts, or accessories thereof. For example, the base material can be made of the same material as the above-mentioned cover material, and in that case, both sides of the clear layer can be formed as ones with high smoothness and good quality. That is, by selecting the base material and the cover material, smoothness can be imparted to only one side or both sides of the single clear layer.

[0098] Furthermore, if a cover material or base material having a relatively large surface roughness is used, a single clear layer having no smoothness can be obtained.

[0099] In addition, the clear layer of the present invention has a simple structure of only one layer, and can be manufactured by a simple method using existing equipment, and does not require complicated and expensive manufacturing such as injection molding, so it is economically advantageous. Furthermore, since the manufacturing process is performed by the flow shown in Figure 1 and aging after the cover material is placed, the amount of clear composition used and the solvent evaporation can be easily controlled and processed, which is excellent from the viewpoint of environmental protection. The same applies to the above-mentioned laminate, composite coating film, and their manufacturing methods, and as a result, composite products such as insert moldings obtained by using them can also be efficiently manufactured.

[0100] The materials used in the laminate of the present invention will be described below.

[0101] [Base material (base film)] The base film is appropriately selected taking into consideration the material to which the composite coating film is applied.

[0102] As a specific example of the base film, a polypropylene composition containing polypropylene (PP) selected from a homopolymer, random copolymer, or block copolymer of polypropylene, or a cured product of a composition containing an acrylonitrile-butadiene-styrene copolymer (ABS resin) can be used. When using a material with low surface wettability such as polypropylene, it is also effective to perform a pretreatment such as a corona treatment or a plasma treatment. By irradiating the surface of the base material with corona discharge or treating it with plasma using a known device, the surface is modified to improve wettability (wet tension), and the repelling of the clear composition from the surface of the base material when applying the primer composition can be prevented in advance.

[0103] In addition, when NH type, NR type (N-alkyl type), or NOR type (N-alkoxyl type) hindered amine (HALS) is added to a polypropylene composition and an ABS resin, the HALS acts as a heat stabilizer, which helps to improve the heat resistance and weather resistance of the object to be coated. It is also advantageous in terms of maintaining the quality of the manufactured laminate when it is stored as is.

[0104] The base film may be colored by adding a coloring agent to the resin material in advance, or may have a colored portion on the surface or inside by printing or the like.

[0105] Furthermore, when the base material is finally peeled off, that is, when the above-mentioned single clear layer is obtained, the coating density is preferably 1.2 to 1.4 g / cm 3It is advisable to use a base material having a water absorption rate of 0.3 to 7.0%, preferably 0.5 to 6.5%, a surface roughness of Ra 1 μm or less, preferably 0.01 μm to 1 μm, more preferably 0.01 μm to 0.1 μm, and a surface pencil hardness of 6B to 4H, preferably 2B to 4H, and particularly preferably 2H to 4H. That is, by using the same material as that described above as a preferred example of the cover material, the solvent remaining in the clear composition can be volatilized during the aging process even on the surface of the base material side, which leads to improving the aesthetics and physical properties of the surface of the clear layer. The mechanism and details of the solvent capture and passage, and the effects thereof have already been described in detail in relation to the cover material.

[0106] Specific examples of base materials that can be peeled off from the clear layer and improve the surface quality of the base material side of the clear layer include cellulose, acetylated cellulose, (meth)acrylic resin, polyamide, porous polypropylene and porous polyethylene, or polyolefin nonwoven fabric.

[0107] [Composition of Solvent-Based Primer Coating Composition] In the present invention, for example, a general primer can be used, which is made of chlorinated polypropylene as a base material, and is made reactive with an epoxy resin and diluted with an organic solvent. In addition, a material that contributes to improving the adhesion between the base material and the clear composition usable in the present invention can be appropriately selected and used from known primers generally used for painting vehicle parts (bumpers, etc.).

[0108] [Composition of Solvent-Based Clear Coating Composition] There is no particular restriction on the clear composition as long as it is a composition that can be cured and formed into a film by the method of the present invention, but in particular, when used as the exterior of an automobile or the like, it is preferable that the clear composition is a material that can produce a clear layer having sufficient hardness, surface quality (appearance), weather resistance, and other properties such as scratch resistance. In this case, any of the compositions for clear coats that have been used conventionally can be used. For example, clear compositions containing acrylic resins, such as poly(meth)acrylate and aminoplast components such as melamine, as resin components, and clear compositions containing poly(meth)acrylate and poly(blocked)isocyanate as resin components can be mentioned. Among these, the clear layer obtained from poly(meth)acrylate and poly(blocked)isocyanate as resin components has particularly excellent scratch resistance, and is therefore extremely preferable for forming a coating film for a substrate used outdoors.

[0109] In particular, the clear composition is preferably a composition mainly composed of an acrylic resin, more specifically, one or more kinds of hydroxyl-containing acrylic resin, particularly hydroxyl-containing (meth)acrylate, and an isocyanate, particularly polyisocyanate. In this specification, (meth)acrylate means either acrylate or methacrylate, poly(meth)acrylate means a polymer containing acrylate or methacrylate, and polyisocyanate means a compound having two or more isocyanate groups per molecule. In addition, a polyurethane solution can be used as the clear composition.

[0110] The clear composition of the present invention preferably contains two types of resins, a hydroxyl-containing (meth)acrylate resin (A) and a hydroxyl-containing (meth)acrylate resin (B) (also referred to as acrylate (A) and acrylate (B)), as the hydroxyl-containing acrylic resin. In this case, the acrylate (A) is a resin having a hydroxyl value of 80 to 220 mgKOH / g, a glass transition temperature of -50°C or higher and lower than 0°C, and containing 25 to 55 mass% of units derived from 4-hydroxybutyl (meth)acrylate in the resin.

[0111] In the present invention, this acrylate (A) can impart sufficient crosslinking density to the coating film, and the clear film (also simply referred to as film) as the cured product of the clear composition has scratch resistance.

[0112] The hydroxyl value of the acrylate (A) is 80 to 220 mgKOH / g, preferably 100 to 200 mgKOH / g, and particularly preferably 120 to 200 mgKOH / g. By making the hydroxyl value 80 mgKOH / g or more, the crosslinking density of the film is sufficiently ensured, the hardness of the film is good, and the stain resistance is improved. In addition, by making the hydroxyl value 220 mgKOH / g or less, the compatibility with the curing agent is good, and the appearance of the film after curing is excellent.

[0113] The acrylate (A) generally contains 25 to 55 mass% of units derived from 4-hydroxybutyl (meth)acrylate, and particularly preferably 30 to 55 mass%. By making the content of 4-hydroxybutyl (meth)acrylate in the acrylate (A) 55 mass% or less, compatibility with the curing agent is improved and the appearance of the film is stabilized.

[0114] The glass transition temperature of the acrylate (A) is −50° C. or higher and lower than 0° C., and preferably −40 to −5° C. A glass transition temperature of −50° C. or higher ensures sufficient film hardness, while a glass transition temperature of 0° C. or lower ensures the mechanical strength of the film.

[0115] In the present invention, the glass transition temperature is measured by DSC, that is, differential scanning calorimetry.

[0116] The acrylate (B) is a resin having a hydroxyl value of 80 to 220 mgKOH / g and a glass transition temperature of 0 to 50° C. By using this acrylate (B) in combination, the obtained film has sufficient crosslink density and hardness.

[0117] The hydroxyl value of the acrylate (B) is 80 to 220 mgKOH / g, preferably 100 to 200 mgKOH / g, and particularly preferably 120 to 200 mgKOH / g. When the hydroxyl value is 80 mgKOH / g or more, sufficient film hardness and stain resistance are obtained. Also, when the hydroxyl value is 220 mgKOH / g or less, compatibility with the curing agent is good, and the appearance of the obtained film is improved.

[0118] The glass transition temperature of the acrylate (B) is 0 to 50° C., and preferably 10 to 50° C. When the glass transition temperature is 0° C. or higher, sufficient film hardness can be obtained, and when the glass transition temperature is 50° C. or lower, the mechanical strength of the film is improved.

[0119] The mass average molecular weight (Mm) of the acrylate (A) and the acrylate (B) is preferably 1,000 to 30,000, more preferably 2,000 to 20,000, and particularly preferably 3,000 to 15,000. When the mass average molecular weight is 1,000 or more, the film hardness is sufficient, and when the mass average molecular weight is 30,000 or less, the compatibility with the curing agent is ensured, resulting in a good film appearance.

[0120] The mass average molecular weights of acrylate (A) and acrylate (B) are molecular weights obtained by GPC (gel permeation chromatography) using polystyrene as a standard polymer, THF as an eluent, and adjusting the sample solution concentration to about 0.1%, using a Tosoh Corporation HLC-8220 GPC in a specified column at a flow rate of 0.35 ml / min, a temperature of 40° C., and a measurement time of 15 minutes. The same applies to the examples described later.

[0121] The acrylate (A) and the acrylate (B) are preferably resins containing 50% by mass or more of units derived from an acrylic monomer, more preferably 70% by mass or more, and particularly preferably 80% by mass or more. It is also preferred that 70% or more, and particularly all, of the hydroxyl groups contained in the acrylate (A) are primary hydroxyl groups.

[0122] In the acrylate (A), the unit derived from the above-mentioned acrylic monomer may be a unit derived from 4-hydroxybutyl (meth)acrylate, and may also contain a unit derived from a radically polymerizable monomer having a primary hydroxyl group. Examples of the radically polymerizable monomer having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, allyl alcohol, 2-hydroxyethyl acrylate, 2-hydroxypropyl acrylate, 3-hydroxypropyl acrylate, 4-hydroxybutyl acrylate, 2-hydroxyethyl methacrylate, 2-hydroxypropyl methacrylate, 3-hydroxypropyl methacrylate, and 4-hydroxybutyl methacrylate with ethylene oxide and / or propylene oxide.

[0123] The acrylate (B) preferably contains a unit derived from a radically polymerizable monomer having a primary hydroxyl group as a unit derived from an acrylic monomer.

[0124] Both the acrylate (A) and the acrylate (B) may contain units derived from other radically polymerizable monomers. Specific examples of other radical polymerizable monomers include methyl acrylate, ethyl acrylate, n-propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, sec-butyl acrylate, hexyl acrylate, cyclohexyl acrylate, 2-ethylhexyl acrylate, octyl acrylate, lauryl acrylate, stearyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, sec-butyl methacrylate, hexyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, octyl methacrylate, lauryl methacrylate, stearyl methacrylate, styrene, acrylonitrile, methacrylonitrile, acrylamide, and methacrylamide. These may be used alone or in a mixture of two or more.

[0125] The acrylate (A) and the acrylate (B) can be produced by radically polymerizing the above radically polymerizable monomers.

[0126] When radical polymerization is carried out to produce the acrylate (A) and the acrylate (B), a radical polymerization initiator may be added to each monomer. Examples of the radical polymerization initiator include azo compounds such as 2,2'-azobisisobutyronitrile, 2.2'-azobis-2,4-dimethylvaleronitrile, 4,4'-azobis-4-cyanovaleric acid, 1-azobis-1-cyclohexanecarbonitrile, dimethyl-2,2'-azobisisobutyrate, methyl ethyl ketone peroxide, cyclohexanone peroxide, 3,5,5-trimethylhexanone peroxide, 1,1-bis(t-butylperoxy)-3,3,5-trimethylcyclohexane, and 1,1-bis(t-butylperoxy)-cyclohexane. Examples of the organic peroxides include 2,2-bis(t-butylperoxy)octane, t-butyl hydroperoxide, diisopropylbenzene hydroperoxide, dicumyl peroxide, t-butyl cumyl peroxide, isobutyl peroxide, lauroyl peroxide, benzoyl peroxide, diisopropyl peroxydicarbonate, t-butyl peroxy 2-ethylhexanoate, t-butyl peroxy neodecanoate, t-butyl peroxy laurate, t-butyl peroxy benzoate, and t-butyl peroxy isopropyl carbonate. The radical polymerization initiator may be used alone or in combination of two or more.

[0127] The amount of the radical polymerization initiator to be added is not particularly limited, but is preferably 0.01 to 20% by mass based on the total amount of the radical polymerizable monomers.

[0128] In these radical polymerization initiator systems, dimethylaniline, ferrous salts such as ferrous sulfate, ferrous chloride, and ferrous acetate, and reducing agents such as sodium acid sulfite, sodium thiosulfate, and Rongalit may be combined as necessary, but it is necessary to select the reducing agent carefully so that the polymerization temperature does not become too low.

[0129] Suitable examples of organic solvents used in the production of acrylate (A) and acrylate (B) include alicyclic hydrocarbon solvents such as cyclohexane and ethylcyclohexane, aromatic hydrocarbon solvents such as toluene, xylene, ethylbenzene, and aromatic naphtha, ketone solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, and isophorone, ester solvents such as ethyl acetate, n-butyl acetate, isobutyl acetate, 3-methoxybutyl acetate, and bis(2-ethylhexyl) adipate, ether solvents such as dibutyl ether, tetrahydrofuran, 1,4-dioxane, and 1,3,5-trioxane, and nitrogen-containing solvents such as acetonitrile, valeronitrile, N,N-dimethylformamide, and N,N-diethylformamide. The organic solvent may be a single solvent or a mixed solvent of two or more types. The solids concentration of the acrylates (A) and (B) can be selected arbitrarily within a range that does not impair the dispersion stability of the resin, but is generally 10 to 90 mass %, preferably 25 to 85 mass %, and more preferably 40 to 80 mass %.

[0130] In producing the acrylate (A) and the acrylate (B), the radical polymerization initiator may be added by any method.

[0131] The acrylate (A) and the acrylate (B) thus obtained can be used either individually or in combination of two or more kinds.

[0132] The content ratio of the hydroxyl group-containing acrylate (A) and the hydroxyl group-containing acrylate (B) in the clear composition of the present invention is in the range of 95 / 5 to 50 / 50, and more preferably in the range of 90 / 10 to 60 / 40, in terms of the solid content mass ratio of the acrylates (A) and (B). By making the acrylate (B) component 5 mass% or more, the chemical resistance of the obtained film is improved, and by making it 50 mass% or less, scratch resistance is obtained.

[0133] The polyisocyanate (curing agent) that can be used as the isocyanate contained in the clear composition of the present invention includes an isocyanate compound having at least two, preferably three or more, isocyanate groups that react with hydroxyl groups in one molecule, and may be used alone or in combination of two or more.

[0134] Examples of polyisocyanate compounds include aromatic diisocyanates such as p-phenylene diisocyanate, biphenyl diisocyanate, tolylene diisocyanate, 3,3'-dimethyl-4,4'-biphenylene diisocyanate, and methylene bis(phenylisocyanate), alicyclic diisocyanates such as isophorone diisocyanate and methylcyclohexyl diisocyanate, linear aliphatic diisocyanates such as 1,4-tetramethylene diisocyanate, hexamethylene diisocyanate, 2,2,4-trimethylhexane-1,6-diisocyanate, lysine methyl ester diisocyanate, bis(isocyanatoethyl) fumarate, and 2-isocyanatoethyl-2,6-diisocyanatohexanoate, as well as biuret compounds and isocyanurates thereof. Isocyanates can be used alone or in combination.

[0135] The clear composition of the present invention preferably contains an aliphatic diisocyanate, including the above-mentioned alicyclic and linear aliphatic diisocyanates, particularly a linear aliphatic diisocyanate, as a curing agent. It is preferable that the curing agent contains 50% by mass or more, preferably 85% by mass or more, and particularly preferably 100% by mass, based on the total amount of isocyanates used. By using a large amount of aliphatic diisocyanate, the film as the cured product of the clear composition has excellent weather resistance, and in particular the gloss of the obtained film surface is maintained for a long period of time.

[0136] The content ratio of the isocyanate group of the isocyanate to the total hydroxyl group of the acrylate (A) and the acrylate (B) is 0.5 to 1.5 in terms of the NCO / OH molar ratio, preferably 0.8 to 1.2. When the NCO / OH molar ratio is less than 0.5 or more, sufficient crosslinking density is obtained, and acid resistance and film hardness are improved. In addition, by making the NCO / OH molar ratio 1.5 or less, weather resistance is improved.

[0137] The clear composition of the present invention further contains an organic solvent. The organic solvent can be any of the organic solvents described above as examples used in the production of the acrylate (A) and the acrylate (B), and can be the same as those used in the production of these. It is possible to use the residual solvent used in the acrylate (A) and the acrylate (B) as a dilution solvent for the clear composition without particularly removing it. That is, it is also possible not to add any organic solvent other than the residual solvent used in the acrylate (A) and the acrylate (B). The organic solvent to be further added may be one type alone or a mixed solvent of two or more types.

[0138] The clear composition of the invention is capable of self-repairing scratches and can form a film with excellent scratch resistance.

[0139] In addition to the above, the clear composition of the present invention may be used by adding one or more of various additives, such as a weathering stabilizer, particularly a weathering stabilizer system (composition) composed of an ultraviolet absorbing agent (UV absorbing agent) and a hindered amine weathering stabilizer, antioxidants, surfactants, surface conditioners, curing reaction catalysts, antistatic agents, fragrances, dehydrating agents, and further rheology adjusters such as polyethylene wax, polyamide wax, and internally crosslinked resin particles, as necessary. Any of these may be appropriately used from known materials.

[0140] Among these, it is preferable to use UV absorber and hindered amine together as weathering stabilizer.When the clear composition of the present invention is used as the outermost layer coating of the exterior of the coating object such as automobile, it may be exposed to all kinds of changes in outdoor weather for a long period of time, and especially in the case of private cars, the gloss and beauty of the appearance may affect the function and value including the durability of the car, so by using the weathering stabilizer in combination (as a composition) as described above, the state of the clear film applied to the coating object can be maintained close to the state at the time of shipment for more than several decades, especially 20 years.

[0141] In particular, it is preferable to add two types of triazine-based ultraviolet absorbers and a NOR-type hindered amine weathering stabilizer (HALS) to the clear composition exemplified as being preferable for application of the present invention. Of these, one of the two types of triazine-based ultraviolet absorbers is a material that absorbs short-wavelength (320 nm or less) ultraviolet rays (hereinafter also referred to as a short-wavelength UV absorber), and the other is a material that absorbs long-wavelength (over 320 nm) ultraviolet rays (hereinafter also referred to as a long-wavelength UV absorber), and since it is possible to absorb ultraviolet rays over a wide range, the quality of the clear film is maintained and the lower layer covered by the clear film is protected from ultraviolet rays.

[0142] The short wavelength UV absorber is preferably an o-hydroxytris-aryltriazine UV absorber of the following formula (1), and the long wavelength UV absorber is preferably an o-hydroxytris-aryltriazine UV absorber of the following formula (2).

[0143] [ka]

[0144] [Wherein, G1 is hydrogen; C1 to C 18 Alkyl; -OH, C2-C 18 alkenyloxy, -C(O)OL1 and -OC(O)L2 (wherein L1 and L2 are independently C1 to C 18C1-C substituted with 1, 2 or 3 groups selected from the group consisting of alkyl, 18 Alkyl; C3-C interrupted by oxygen 50 Alkyl; or C3-C interrupted by oxygen 50 is hydroxyalkyl, G2, G3, G4 and G5 are independently hydrogen; 18 alkyl; phenyl; or phenyl substituted with 1, 2 or 3 C1-C4 alkyl.

[0145] [ka]

[0146] [In the formula, Q1, Q2, Q3 and Q4 are independently hydrogen; 18 Alkyl; -OH, C2-C 18 alkenyloxy, -C(O)OY and -OC(O)Y (wherein Y and Y are independently C1 to C2 18 C1-C substituted with 1, 2 or 3 groups selected from the group consisting of alkyl, 18 Alkyl; C3-C interrupted by oxygen 50 Alkyl; or C3-C interrupted by oxygen 50 is hydroxyalkyl, R 14 , R 15 and R 16 are each independently hydrogen or C1-C 18 is alkyl]

[0147] Among the o-hydroxytris-aryltriazine UV absorbers of formula (1), the following compounds are particularly preferably used:

[0148] [ka] TIFF0007567046000004.tif125150 TIFF0007567046000005.tif163150

[0149] Among the o-hydroxytris-aryltriazine UV absorbers of formula (2), the following compounds are particularly preferably used:

[0150] [ka]

[0151] The long-wavelength UV absorbent and the short-wavelength UV absorbent may each be one type of compound or a mixture of multiple types. Commercially available examples of long-wavelength UV absorbents include Tinuvin (registered trademark), 460, 477, 479, 970, 1600 (manufactured by BASF Japan Ltd.) and ADK STAB (registered trademark) LA-F70 (manufactured by ADEKA Corporation). Commercially available examples of short-wavelength UV absorbents include Tinuvin (registered trademark) 400, 405, 1577 (manufactured by BASF Japan Ltd.) and ADK STAB (registered trademark) LA-46 (manufactured by ADEKA Corporation).

[0152] These ultraviolet absorbents have a long life as compounds themselves and protect the composition to which they are added, and further provide good protection for the objects to be coated therewith (primer layers, base materials and substrates, printing inks and pigments).

[0153] The NOR type hindered amine light stabilizer generally has a molecular weight of more than 200 g / mol, preferably more than 500 g / mol, particularly more than 700 g / mol, more preferably more than 700 g / mol to 10,000 g / mol, for example, up to 50,000 g / mol. A molecular weight of 700 g / mol to 5,000 g / mol is particularly preferred.

[0154] The NOR type hindered amine light stabilizer is represented by the formula (3): [ka] [In the formula, E1 is C1~C18 Alkoxy; Hydroxy substituted C1-C 18 Alkoxy; m1 is 1, 2 or 4; When m1 is 1, E2 is C1 to C 25 an alkyl group, a group of the formula -C(CH3)=CH2, or a group of the formula (3a): [ka] wherein E3 is as defined for E1. Based on When m1 is 2, E2 is C1 to C 14 Alkylene, or formula (3b): [ka] (In the formula, E4 is C1~C 10 Alkyl or C2-C 10 alkenyl, E5 is C1~C 10 alkylene, and E6 and E7 are each independently C1-C4 alkyl, cyclohexyl, or methylcyclohexyl. and When m1 is 4, E2 is C4-C 10 Alkanetetrayl] The compound is used. One or more types of NOR type hindered amine light stabilizers may be added. Commercially available products include TINUVIN (registered trademark) 123, 144, 765, and 770 (manufactured by BASF Japan Ltd.), and ADK STAB (registered trademark) LA-81, 82, and 87 (manufactured by ADEKA Corporation).

[0155] Such NOR-type hindered amine light stabilizers have the role of protecting the composition to which they are added from heat, light, and chemical substances from the outside world. Therefore, when the NOR-type hindered amine light stabilizer is contained, the clear film of the present invention containing the same is less susceptible to the influence of external environments such as acid rain, and internal environments such as acidic atmospheres associated with resin deterioration. Furthermore, such hindered amine light stabilizers can provide the film with thermal stability over the long period during which the substrate to be coated, such as an automobile, maintains its function.

[0156] As another UV absorbent, ADK STAB (registered trademark) LA-1000 (manufactured by ADEKA Corporation) can also be used.

[0157] The clear film of the present invention is preferably used as a topcoat constituting the outermost coating of the object to be coated, but it can also be used as a colored film by blending a colorant such as a dye or pigment.

[0158] The clear composition of the present invention may be either one-component type or two-component type. In order to obtain the laminate of the present invention, it is convenient to use the two-component type without complicating the process by using a blocked isocyanate or the like, and this allows the film to have excellent physical properties and surface quality.

[0159] According to the manufacturing method of the present invention, a laminate having a clear layer with excellent appearance and mechanical properties, a composite layer, and a single layer of a clear layer can be obtained by directly applying a cover material having a predetermined property onto the clear composition. This is because the solvent in the clear composition is well removed through the above-mentioned predetermined cover material, the burden on the environment is suppressed, and the manufacturing process is simple and efficient. By using the cover material and clear composition listed as the above-mentioned preferred examples, it is possible to maintain the physical properties and surface state of the clear layer in an optimal state. It is impossible or impractical to further specify the properties and surface state of the obtained clear layer by other than the physical properties or structure of each material described in the manufacturing method including the above-mentioned steps, because it requires extremely detailed analysis. The same applies to the clear layer that forms the surface of a molded body such as an insert molded body.

[0160] In addition, the clear layer obtained by the present invention has a surface formed by contacting the clear composition with the cover material having the above-mentioned specified characteristics (both surfaces in the case of a single-layer clear layer formed by sandwiching both surfaces between a cover material having the above-mentioned specified characteristics and a base material having similar characteristics) that has extremely excellent smoothness. In the present invention, it is possible to achieve a surface quality of the clear layer that is at least twice, preferably at least 10 times, smoother than the coating film obtained by general spray painting or the like.

[0161] In addition, the laminate or composite coating film of the present invention is applied to a substrate (subject to be coated) made of synthetic resin, but the present invention is not limited to this. For example, the laminate or composite coating film of the present invention can be applied to metals such as aluminum and stainless steel, CFRP (carbon fiber reinforced plastic), etc.

[0162] Specific examples of objects to be coated to which the laminate or composite coating film of the present invention can be applied include automobiles (vehicle bodies or parts thereof), automobile parts (e.g., bodies, bumpers, spoilers, mirrors, wheels, interior materials, and other parts made of various materials), motorcycles, motorcycle parts, bicycles, bicycle parts (e.g., frames, handlebars, spoilers, mirrors), road materials (e.g., guardrails, traffic signs, soundproof walls, etc.), ships, railway vehicles, aircraft, buildings, construction materials, furniture, home appliances, containers, musical instruments, office supplies, sporting goods, toys, and parts or portions thereof.

[0163] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. In the following, unless otherwise specified, "parts" and "%" are based on mass. EXAMPLES

[0164] [Production Example 1] Preparation of hydroxyl-containing resin solution, A-1 33.9 parts of xylene was charged into a four-neck flask equipped with a thermometer, a reflux condenser, a stirrer, and a dropping funnel, and the mixture was heated to 140°C while stirring under a nitrogen stream. Next, at a temperature of 140°C, a mixture of 12 parts of styrene, 24 parts of cyclohexyl methacrylate, 24 parts of 4-hydroxybutyl acrylate, and 5 parts of t-butylperoxy-2-ethylhexanoate as a polymerization initiator was uniformly mixed and dropped from the dropping funnel over 2 hours. After the drop was completed, the temperature was kept at 140°C for 1 hour, and then the reaction temperature was lowered to 110°C. Then, a polymerization initiator solution in which 0.1 parts of t-butylperoxy-2-ethylhexanoate was dissolved in 1 part of xylene as a polymerization initiator was added as an additional catalyst, and the reaction was terminated when the temperature of 110°C was kept for 2 hours, to obtain a hydroxyl group-containing resin solution A-1.

[0165] [Table 1]

[0166] [Production Example 2] Preparation of hydroxyl-containing resin solution, B-1 A hydroxyl-containing resin solution B-1 was obtained in the same manner as in A-1, except that the amounts of the raw materials were changed to those shown in Table 2.

[0167] [Table 2]

[0168] [Production Example 3] Preparation of clear composition CC-1 The raw materials shown in Table 3 were mixed in order and stirred until homogeneous to prepare clear composition CC-1. The amount of each component shown in Table 3 is in parts by mass. The unit of Tg is °C.

[0169] [Table 3]

[0170] Table Notes Desmodur N3300: Product name, manufactured by Sumika Covestro Urethane Co., Ltd., liquid HDI nurate type resin (solid content 100%, NCO content 23% by mass) UV absorber solution: 20% by mass solution of Tinuvin 900 and Tinuvin 479 (trade names, manufactured by BASF Japan) in xylene Light stabilizer solution: 20% by mass solution of Tinuvin 292 and Tinuvin 123 (trade names, manufactured by BASF Japan) in xylene Surface conditioner solution: 10% by weight of BYK-300 (product name, manufactured by BYK-Chemie) in xylene Solvesso 100: Product name, aromatic petroleum naphtha, manufactured by Esso Corporation

[0171] [Examples 1 to 3, Comparative Examples 1 to 3] <Preparation of samples for evaluation in Examples 1 to 3 and Comparative Examples 1 to 3> A 100 μm thick black cast polypropylene (CPP) that had been corona-treated was placed on a horizontal table. The CPP was used as a base material, and a primer was applied to the corona-treated surface of the base material to a thickness of 5 μm and dried in an oven at 150 ° C for 5 minutes. A clear composition, CC-1, was applied to the dried primer on the base material with a table coat to a film thickness of 25 μm to provide a clear composition layer. Next, a cover material was attached to the upper surface of the clear composition before drying (the side opposite to the base material) so as to be in close contact with the clear composition. The four-layered film of the resin layer on the base material obtained in this way was heated and dried for 4 days in an oven at 40 ° C. It was confirmed that there were no dents in the resin layer, that there were no air bubbles or air layers between the resin layer and the cover film, and that the cover material covered the entire upper surface of the resin layer. As the above cover material, TAC film, Fujitac FTTG60UL (manufactured by Fuji Film Corporation) was used.

[0172] The four-layered film obtained as described above was cut into a 10 cm square, and all edges of the resulting square film, i.e., the entire periphery, were covered with aluminum tape to seal the edges so that the solvent in the resin layer would not volatilize.

[0173] The type and content (solid content) of the solvent in the above clear composition CC-1 and the type of the cover film were changed as shown in Table 1 below to obtain samples of Examples 1 to 3 and Comparative Examples 1 to 3.

[0174] When a polypropylene film was used as the cover material, the clear composition could not be held between the polypropylene film and the base material, and a four-layer film could not be obtained.

[0175] <Aging characteristic evaluation> The samples of the examples and comparative examples were placed in a thermostatic chamber at 40°C and subjected to aging treatment. The mass of the sample immediately before being placed in the thermostatic chamber was measured using an analytical electronic balance. Furthermore, the mass of the sample during the aging treatment was measured after 1 day, 2 days, 3 days, 5 days, and 7 days using the same analytical electronic balance as above to determine the mass change (mass difference due to volatilization of residual solvent). Furthermore, the resin layers of the present invention in Examples 1 to 3 were completely cured within 3 days, whereas the resin layers of Comparative Examples 1 to 3 required 7 days even though the same resin material was used.

[0176] <Removability evaluation> The cover films were manually peeled off from both the example samples and the comparative sample cured as described above on the seventh day after the start of aging. The same test was repeated three times, and the peelability was evaluated according to the following criteria.

[0177] The cover film is easily peelable. ×: The resin layer was stuck to the cover film and was difficult to peel off.

[0178] <Surface characteristic evaluation> After the peel test, the surface condition of the samples of the examples and comparative examples was visually evaluated according to the following criteria.

[0179] After peeling, no roughness or irregularities were observed on the surface of any of the three samples, and a smooth and glossy surface was obtained. ×: Roughness or irregularities such as unevenness or scratches were observed on the surfaces of the three samples after peeling, and the gloss was lost.

[0180] The results of each of the above tests are shown in Table 1.

[0181] [Table 4]

[0182] In addition, the values ​​for each day in Table 4 indicate values ​​measured at each time point, with 24 hours from the start of the aging treatment being defined as 1 day.

[0183] Furthermore, the expressions in Table 4 have the following meanings.

[0184] Composition 1: Clear composition CC-1 in xylene (solid content 49%) Composition 2: Clear composition CC-1 in xylene (solids content 80%) Composition 3: Clear composition CC-1 in butyl acetate (solids content 49%) TAC: Triacetyl cellulose (density: 1.22-1.34 g / cm 3 , water absorption rate 1.7-6.5% (water absorption rate when in contact with the clear composition surface for 24 hours), surface roughness Ra 0.01μm-0.1μm, surface pencil hardness 2H) Surface-treated PET: Polyethylene terephthalate surface-treated with a silicone release layer (density: 1.34-1.39 g / cm 3 , water absorption rate 0.10-0.20% (water absorption rate when in contact with the clear composition surface for 24 hours), surface roughness Ra 0.1 μm, surface pencil hardness HB)

[0185] In the examples according to the present invention, the resin layer as the clear layer allowed the organic solvent to be removed well in a much shorter time than in the comparative examples, and aging and curing were also shown to be performed well. In addition, in the laminate of the examples of the present invention, the cover film from the clear layer after curing was formed more quickly than the film using the release agent of the comparative example, even though no release agent treatment was performed. Furthermore, the surface quality of the obtained clear layer was also extremely high, and it was observed that the haze was reduced and the smoothness and gloss were significantly improved compared to the surface obtained in the comparative example.

[0186] [Example 4, Comparative Example 4] <Creating laminated film> Using the clear composition CC-1 (solvent: 35.1 parts, solid content: 114.9 parts), the clear composition was applied to a base material (film thickness 460 μm) at a film thickness of 60 μm (film thickness after drying: 30 μm), and the total thickness of the laminate was set to 520 μm (film thickness after drying: 490 μm). Except for this, the laminate film for evaluation in Example 4 was produced using the same method as the production of the sample in Example 1 described above. The film thickness of the laminate film after drying was 490 μm.

[0187] <Molding of an insert molded article sample for evaluation in Example 4> A film insert molded sample plate (150mm x 150mm square) was prepared using an injection molding machine J220ADS-300H manufactured by Japan Steel Works, Ltd. That is, the sample of Example 4 obtained as described above was cut into a 70mm x 150mm square, the cover film was peeled off, and the clear layer side of the laminate film was aligned so as to be placed in the center of the inner surface of the mold (#3000) and fixed with cellophane tape (registered trademark), and polypropylene, which is a resin constituting the base, was introduced to the base material side using an injection molding device. By cooling at a mold temperature of 80 ° C. for 25 seconds, the base film and the polypropylene base were fused and integrated, and a 150mm square injection molded plate (insert molded product) with a thickness of 3 mm was obtained.

[0188] <Production of sample by spray painting for evaluation in Comparative Example 4> The sample of Comparative Example 4 was prepared by cutting a standard painted molded product into a square of 70 mm x 150 mm. This sample was prepared by providing a clear layer by conventional spray painting as the outermost layer on a substrate used as an exterior part of an automobile. The clear layer of Comparative Example 4 had the highest level of surface quality that has been conventionally applied to luxury cars.

[0189] <Measurement of smoothness> The surface smoothness of the clear layer of the samples of Example 4 and Comparative Example 4 was measured in accordance with JIS B 0601 using a Wavescan II (Cat. No. 4846, manufactured by BYK-Gardner).

[0190] The measurement results are shown in Table 5.

[0191] [Table 5]

[0192] Furthermore, the smoothness of the clear layer surface of the sample of Example 4 and Comparative Example 4 was measured using a stylus surface profiler (Dektak 6M stylus profiler, manufactured by Veeco). In this test, an operator randomly selected five points on the surface of the clear layer of each sample of Example 4 and Comparative Example 4 to measure the surface roughness (Ra: arithmetic mean roughness, and Rq: root mean square). The measurement results of the five arbitrary points are designated as measurements 1 to 5, and are shown in Table 6 together with their average values.

[0193] The differences in smoothness and gloss between the samples of Example 4 and Comparative Example 4 were clear even by visual observation, and all 10 observers recognized that the smoothness and gloss of the sample of Example 4 were far superior to the sample of Comparative Example 4. On the other hand, the same observers also visually observed that there was no unevenness in either roughness or gloss on the clear layer surfaces of the samples of Example 4 and Comparative Example 4, and it was recognized that no matter which position was measured and averaged, it would not have a significant effect on the measured values.

[0194] [Table 6]

[0195] The above data for Example 4 are comparable to the coating of Comparative Example 4 obtained by spray coating and then finish polishing (mirror finish).

[0196] Furthermore, when the samples according to the examples of the present invention and the comparative examples were subjected to predetermined weather resistance, chemical resistance, and damage resistance tests, good results were obtained in these tests as well.

[0197] The invention made by the present inventors has been specifically described above based on an embodiment, but it goes without saying that the present invention is not limited to the above embodiment and can be modified in various ways without departing from the gist of the invention. [Explanation of symbols]

[0198] 1 Roll lamination device 10, 120 base film 12 Roll coater device 14 Clear composition 18, 150 Cover film 100 Laminate 200 Base

Claims

1. A solvent-based clear coating composition is applied onto a base material; A cover material is placed on the solvent-based clear coating composition while the solvent-based clear coating composition is in an uncured state; The method includes the steps of subjecting the uncured laminate composed of the base material, the solvent-based clear coating composition, and the cover material obtained by the above-mentioned process to an aging treatment to cure the uncured solvent-based clear coating composition and form a cured laminate including a cured clear layer, A method for producing a laminate, characterized in that the cover material is a material that captures and passes through the solvent in the solvent-based clear coating composition.

2. The cover material has a density of 0.09 to 1.4 g / cm 3 2. The method for producing a laminate according to claim 1, characterized in that the laminate is made of a resin having a water absorption rate of 0.3 to 7.0%, a surface roughness Ra of 1 μm or less, and a pencil hardness of 6B to 4H.

3. A solvent-based primer coating composition is applied on the base material in advance, Applying the solvent-based clear coating composition onto the solvent-based primer coating composition; A cover material is placed on the solvent-based clear coating composition while the solvent-based clear coating composition is in an uncured state; The method for producing a laminate according to claim 1 or 2, further comprising subjecting the uncured laminate thus obtained, which is composed of the base material, the solvent-based primer coating composition, the solvent-based clear coating composition, and the cover material, to the aging treatment.

4. The method according to any one of claims 1 to 3, further comprising the step of winding the uncured laminate into a wound body, and subjecting the wound body to the aging treatment.

5. The method according to any one of claims 1 to 4, wherein the cover material is cellulose, acetylated cellulose, (meth)acrylic resin, polyamide, porous polypropylene and porous polyethylene, or a polyolefin nonwoven fabric.

6. The method according to any one of claims 1 to 5, wherein the solvent-based clear coating composition is a composition containing one or more hydroxyl group-containing (meth)acrylic resins and an isocyanate crosslinking agent, or a composition containing a urethane polymer solution.

7. The method according to claim 6, wherein the solvent-based clear coating composition further comprises a weathering stabilizer.

8. The method according to any one of claims 1 to 7, wherein the base material is a cured product of a composition containing a propylene homopolymer, random copolymer or block copolymer, or an acrylonitrile-butadiene-styrene copolymer.

9. The method of claim 8, wherein the composition comprises a hindered amine weathering stabilizer.

10. The base material has a density of 0.09 to 1.4 g / cm 3 The method according to any one of claims 1 to 7, wherein the resin has a water absorption rate of 0.3 to 7.0%, a surface roughness Ra of 1 µm or less, and a pencil hardness of 6B to 4H.

11. The method according to claim 10, wherein the base material is cellulose, acetylated cellulose, (meth)acrylic resin, polyamide, porous polypropylene and porous polyethylene, or a polyolefin nonwoven fabric.

12. A laminate comprising the base material, the cured clear layer, and the cover material, the laminate being obtained by the manufacturing method according to any one of claims 1 to 9.

13. A method for producing a composite coating film, comprising: producing a composite coating film comprising the base material and the cured clear layer by removing the cover material from the laminate according to claim 12.

14. A composite coating film obtained by the method according to claim 13.

15. A method for producing a molded article, comprising applying the composite coating film according to claim 14 to a substrate to produce a molded article having the clear layer.

16. The method for producing a molded article according to claim 15, characterized in that the molded article is molded by insert molding the composite coating film onto the substrate, and has the clear layer as an outermost coating layer.

17. 17. The method according to claim 15 or 16, wherein the substrate is selected from the group consisting of automobiles, motorcycles, bicycles, road materials, ships, railroad vehicles, aircraft, buildings, construction materials, furniture, home appliances, containers, musical instruments, office supplies, sporting goods, toys, and parts or portions thereof.

18. A molded article obtained by the method according to any one of claims 15 to 17.

19. A laminate comprising the base material, the cured clear layer, and the cover material, the laminate being obtained by the manufacturing method according to claim 10 or 11.

20. A clear layer obtained by removing the base material and the cover material from the laminate according to claim 19.

Citation Information

Patent Citations

  • Molding method of thermoformable laminated sheet and molded product

    JP2005169654A

  • Method for manufacturing laminated sheet

    JP2005335161A

  • Laminated sheet for shaping and its production method

    JP2006062231A

  • Molding method of thermoforming laminated sheet and molded product

    JP2006341388A

  • Automobile interior trim material and automobile interior part

    JP2008110651A