Large sintered yttrium oxide bodies
High-purity, high-density sintered yttrium oxide bodies with controlled porosity and impurity levels, produced via spark plasma sintering, address the limitations of existing materials by enhancing etch resistance and mechanical strength in plasma etch chambers, reducing contamination and process drift.
Patent Information
- Application Number
- JP2023519271
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-11
- Filing Date
- 2021-09-30
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2041-09-30
AI Technical Summary
Existing sintered yttrium oxide materials suffer from low sintering strength, porosity, and adhesion issues, limiting their use in large-scale plasma etch chambers due to erosion and corrosion, which leads to increased tool downtime, contamination, and process drift.
The development of high-purity, high-density sintered yttrium oxide bodies with controlled pore sizes and impurity levels, manufactured through spark plasma sintering using specific tool parameters, resulting in enhanced mechanical strength and resistance to plasma etching.
The solution provides improved etch resistance, reduced particle generation, and extended component life in plasma etch chambers, minimizing contamination and process drift, while maintaining uniformity and mechanical integrity.
Smart Images

Figure 0007567048000023 
Figure 0007567048000024 
Figure 0007567048000025
Abstract
Description
[Technical field]
[0001] The present disclosure relates to high purity, high density sintered yttrium oxide bodies having properties that lead to superior etch resistance when used as components in plasma etch chambers. Additionally, the present disclosure provides processes for making the sintered yttrium oxide bodies. [Background technology]
[0002] In the field of semiconductor material processing, vacuum processing chambers are used for etching and chemical vapor deposition (CVD) of materials on substrates. A process gas is introduced into the processing chamber while a radio frequency (RF) field is applied to the process gas to generate a plasma of the process gas.
[0003] During processing of semiconductor substrates, the substrate is typically supported in a vacuum chamber by a substrate holder, as disclosed, for example, in U.S. Patent Nos. 5,262,029 and 5,838,529. Process gases can be supplied to the chamber by a variety of gas delivery systems. Other equipment used in processing semiconductor substrates includes windows, nozzles, showerheads, (etch) chamber liners, mixing manifolds, wafer supports, electronic wafer chucks, and various rings, such as focus rings and guard rings, among other components.
[0004] In such processes, plasma is typically used to remove material on the chamber walls and substrate. Plasma etch conditions produce significant ion bombardment of the surfaces of the processing chamber exposed to the plasma. This ion bombardment, combined with plasma chemicals and / or etch by-products, can cause significant surface roughening, erosion, corrosion, and corrosion-erosion of the plasma-exposed surfaces of the processing chamber. As a result, surface material is removed by physical and / or chemical attack. This attack causes problems including extended tool downtime, increased consumable costs, particulate contamination, transition metal contamination on the wafer, and short parts life resulting in process drift.
[0005] Additionally, plasma processing chambers have been designed to include components such as disks, rings, and cylinders that confine the plasma above the wafer being processed. However, these components used in plasma processing chambers are continually attacked by the plasma and as a result, they erode or accumulate contaminants and polymer deposits.
[0006] Due to the erosive and corrosive nature of the plasma environment in such reactors, there is a need to minimize particle and / or metal contamination. It is therefore desirable for the components of such equipment, including consumables and other parts, to have suitably high erosion and corrosion resistance. Such parts have been formed from materials that provide resistance to corrosion and erosion in the plasma environment, as described, for example, in U.S. Patent No. 5,798,016, U.S. Patent No. 5,911,852, U.S. Patent No. 6,123,791, and U.S. Patent No. 6,352,611.
[0007] Yttrium oxide is known to exhibit significantly higher resistance to halogen-based corrosive gases and the plasmas of such gases compared to other common ceramic materials such as alumina, silicon carbide, silicon nitride, and zirconia, and therefore, yttrium oxide is commonly applied as a layer to corrosion-resistant components in semiconductor manufacturing equipment involving plasma processing.
[0008] However, the use of yttrium oxide has drawbacks. Yttrium oxide has persistent problems such as low sintering strength that hinders its development as a structural material in these plasma-resistant applications. Low sintering strength can also be a limiting factor for making large parts due to breakage as the component size increases. For this reason, in some cases, yttrium oxide can be used as a coating for corrosion-resistant components, and the components are manufactured by spraying yttrium oxide onto a substrate made of a metal material that is cheaper and stronger than yttrium oxide, or a ceramic material made of other materials such as alumina.
[0009] However, yttrium oxide materials still suffer from many drawbacks in plasma etching processes, such as significant porosity in the yttria coating and reduced adhesion strength between the yttria and the base layer. The presence of porosity in the coating would adversely affect the corrosion and erosion resistance of the components. Furthermore, yttrium oxide is difficult to sinter by conventional methods, especially to form sintered bodies of large dimensions. As a result, there is a need for yttrium oxide materials for use in plasma etching chambers that do not suffer from such drawbacks. Summary of the Invention
[0010] These and other needs are addressed by the various embodiments, aspects, and configurations disclosed herein.
[0011] Total impurity level of 140 ppm or less, 4.93 g / cm 3 The density is 1 atom / nm2 to 10 atoms / nm 2 1. A sintered yttrium oxide body having at least one grain boundary containing an amount of silica below 0.01% and having at least one surface containing at least one pore, each pore being 5 μm or less in diameter.
[0012] Embodiment 2 Density is 4.96 g / cm 3The sintered yttrium oxide body according to embodiment 1 is as described above.
[0013] Embodiment 3: Density is 4.98 g / cm 3 The sintered yttrium oxide body according to any one of the first and second embodiments described above.
[0014] Embodiment 4 Density is 5.01 g / cm 3 The sintered yttrium oxide body according to any one of embodiments 1, 2 or 3.
[0015] Embodiment 5. A sintered yttrium oxide body according to any one of embodiments 1 to 4, wherein all pores have a diameter of 4 μm or less.
[0016] Embodiment 6. A sintered yttrium oxide body according to any one of embodiments 1 to 5, wherein all pores have a diameter of 3 μm or less.
[0017] Embodiment 7. A sintered yttrium oxide body according to any one of embodiments 1 to 6, wherein all pores have a diameter of 2 μm or less.
[0018] Embodiment 8. A sintered yttrium oxide body according to any one of embodiments 1 to 7, wherein all pores have a diameter of 1 μm or less.
[0019] Embodiment 9. The sintered yttrium oxide body of any one of embodiments 1-8, having a total impurity level of 35 ppm or less.
[0020] Embodiment 10. The sintered yttrium oxide body of any one of embodiments 1-9, having a total impurity level of 30 ppm or less.
[0021] Embodiment 11. The sintered yttrium oxide body of any one of embodiments 1-10, having a total impurity level of 25 ppm or less.
[0022] Embodiment 12. The sintered yttrium oxide body of any one of embodiments 1-11, having a total impurity level of 20 ppm or less.
[0023] Embodiment 13. The sintered yttrium oxide body of any one of embodiments 1-12, having a total impurity level of 15 ppm or less.
[0024] Embodiment 14. The sintered yttrium oxide body of any one of embodiments 1-13, having a total impurity level of 10 ppm or less.
[0025] 1.5×10 at 1 MHz, measured at ambient temperature according to ASTM D150 -2 ~5.0×10 -2 15. The sintered yttrium oxide body according to any one of the preceding embodiments, having a dielectric loss of
[0026]
[0036] In a process in which a 10 mm x 5 mm area of at least one surface is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power, a 375,000 μm 3 16. The sintered yttrium oxide body of any one of the preceding claims, wherein the body exhibits an etch volume of less than 100 nm, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm for 1500 seconds, and the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, the first step and the second step being repeated successively until the time of CF4 exposure in the first step is 24 hours.
[0027] Embodiment 17: Approximately 325,000 μm 3 17. The sintered yttrium oxide body of any one of the preceding embodiments, wherein the sintered yttrium oxide body exhibits an etch volume of less than 100 nm.
[0028] Embodiment 18: Approximately 275,000 μm 318. The sintered yttrium oxide body of any one of the preceding embodiments, exhibiting an etch volume of less than 100 nm.
[0029] Embodiment 19. The sintered yttrium oxide body of any one of embodiments 1 to 18, having a pore size distribution with a maximum pore size of 1.50 μm for 95% or more of all pores on at least one surface.
[0030] Embodiment 20. The sintered yttrium oxide body of any one of embodiments 1 to 19, having a pore size distribution with a maximum pore size of 1.75 μm for 97% or more of all pores on at least one surface.
[0031] Embodiment 21. A sintered yttrium oxide body according to any one of embodiments 1 to 20, having a pore size distribution with a maximum pore size of 2.00 μm for 99% or more of all pores on at least one surface.
[0032] Embodiment 22. The sintered yttrium oxide body of any one of embodiments 1-21, wherein a 10 mm×5 mm area of at least one surface exhibits an etch rate of less than about 1.0 nm / min in a process subjected to etching conditions of a pressure of 10 mTorr, an argon flow rate of 20 sccm, a bias of 600 volts, and an ICP power of 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm for 1500 seconds, and the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, the first step and the second step being repeated successively until the time of CF4 exposure in the first step is 24 hours.
[0033] Embodiment 23. The sintered yttrium oxide body of any one of embodiments 1 to 22, having an etching rate of less than 0.9 nm / min.
[0034] Embodiment 24. The sintered yttrium oxide body of any one of embodiments 1 to 23, having an etching rate of less than 0.8 nm / min.
[0035] In the non-etched area, the thickness is 250×10 as determined by ISO standard 25178-2-2012, section 4.3.2. -5 25. The sintered yttrium oxide body of any one of the preceding embodiments, exhibiting a developed interfacial area Sdr of less than 100 nm.
[0036] Embodiment 26: The developed interface area in the non-etched region is 225×10 -5 26. The sintered yttrium oxide body of any one of embodiments 1 to 25, wherein the yttrium oxide body has a thickness of less than 100 nm.
[0037] Embodiment 27: The developed interface area in the non-etched region is 200×10 -5 27. The sintered yttrium oxide body of any one of the preceding embodiments, wherein the yttrium oxide body has a melting point of less than 100 nm.
[0038]
[0046] In a process of subjecting a 6 mm x 6 mm area of at least one surface to etching conditions of 10 mTorr pressure, 90 sccm CF4 flow rate, 30 sccm oxygen flow rate, 20 sccm argon flow rate, and 600 volt bias and 2000 watts ICP power for a duration of 24 hours, the etching area is 200 x 10 -5 28. The sintered yttrium oxide body of any one of the preceding embodiments, exhibiting a developed interfacial area of less than 100 nm.
[0039] Embodiment 29: The developed interface area in the etching region is 175×10 -5 29. The sintered yttrium oxide body of any one of the preceding embodiments, wherein the yttrium oxide body has a melting point of less than 100 nm.
[0040] Embodiment 30: The developed interface area in the etching region is 150×10 -5 30. The sintered yttrium oxide body of any one of the preceding embodiments, wherein the yttrium oxide body has a melting point of less than 100 nm.
[0041] 31. The sintered yttrium oxide body of any one of the preceding claims, wherein a 10 mm x 5 mm area of at least one surface exhibits an arithmetic mean height Sa of less than 30 nm as determined by ISO standard 25178-2-2012, section 4.1.7, in a process subjected to etching conditions of a pressure of 10 mTorr, an argon flow rate of 20 sccm, and an ICP power of 600 volts and 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm for 300 seconds, and the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and steps 1 and 2 are repeated consecutively for a total etching time of 6 hours.
[0042] Embodiment 32. The sintered yttrium oxide body of any one of embodiments 1 to 31, wherein Sa is less than 20 nm.
[0043] Embodiment 33. The sintered yttrium oxide body of any one of embodiments 1 to 32, wherein Sa is less than 15 nm.
[0044] Embodiment 34. The sintered yttrium oxide body of any one of embodiments 1 to 33, wherein at least one surface has an area that is less than 0.15% occupied by pores.
[0045] Embodiment 35. The sintered yttrium oxide body of any one of embodiments 1 to 34, wherein at least one surface has an area that is less than 0.10% occupied by pores.
[0046] Embodiment 36. A sintered yttrium oxide body according to any one of embodiments 1 to 35, exhibiting a step change of 0.27 to 0.28 μm after an SF6 etching process.
[0047] Embodiment 3. A sintered yttrium oxide body according to any one of embodiments 1 to 36, having a particle size d50 of 0.1 μm to 25 μm.
[0048] Embodiment 3: A sintered yttrium oxide body according to any one of embodiments 1 to 37, having a particle size d50 of 80.5 μm to 15 μm.
[0049] Embodiment 39. A sintered yttrium oxide body according to any one of embodiments 1 to 38, having a particle size d50 of 0.5 μm to 10 μm.
[0050] Embodiment 40. The sintered yttrium oxide body of any one of embodiments 1 to 39, having at least one dimension between 100 mm and 600 mm.
[0051] Embodiment 41. The sintered yttrium oxide body of any one of embodiments 1 to 40, having at least one dimension between 100 mm and 406 mm.
[0052] Embodiment 42 The sintered yttrium oxide body of any one of embodiments 1 to 41 having at least one dimension between 200 mm and 600 mm.
[0053] Embodiment 43. The sintered yttrium oxide body of any one of embodiments 1 to 42, having at least one dimension between 350 mm and 600 mm.
[0054] Embodiment 44. The sintered yttrium oxide body of any one of embodiments 1 to 43, having at least one dimension between 500 mm and 600 mm.
[0055] Embodiment 45. The sintered yttrium oxide body of any one of embodiments 1 to 44, having at least one dimension between 550 mm and 600 mm.
[0056] Embodiment 46. The sintered yttrium oxide body of any one of embodiments 1-45, wherein the density does not vary by more than 3% along at least one dimension.
[0057] Embodiment 47. The sintered yttrium oxide body of any one of embodiments 1 to 46, wherein the density does not vary by more than 2% along at least one dimension.
[0058] Embodiment 48. The sintered yttrium oxide body of any one of embodiments 1-47, wherein the density does not vary by more than 1% along at least one dimension.
[0059] Embodiment 49 A process for producing a sintered yttrium oxide body, comprising: a) disposing yttrium oxide powder within an interior volume defined by a spark plasma sintering tool, the spark plasma sintering tool including a die including a sidewall including an inner wall having a diameter defining the interior volume, and an outer wall, and an upper punch and a lower punch operatively coupled to the die, each of the upper punch and the lower punch having an outer diameter smaller than the diameter of the inner wall of the die, whereby when at least one of the upper punch and the lower punch is moved within the interior volume of the die, each of the upper punch and the lower punch and the die are in contact with each other. a) a punch having an inner wall and an upper punch and a lower punch having a width of 10 μm to 70 μm, the gap creating a vacuum within the inner volume; b) applying a pressure of 10 MPa to 60 MPa to the yttrium oxide powder by moving at least one of the upper punch and the lower punch within the inner volume of the die while heating to a sintering temperature of 1200 to 1600° C. to form a sintered yttrium oxide body; and c) reducing the temperature of the sintered yttrium oxide body, the yttrium oxide powder of step a) being sintered to a pressure of 10 MPa to 60 MPa to form a sintered yttrium oxide body. 2 The sintered yttrium oxide body has a surface area of 4.93 g / cm3 or less and a total impurity level of 40 ppm or less. 3 and c) providing a sintered yttrium oxide body having a density of at least 100% or greater, at least one surface containing at least one pore, each pore having a diameter of 5 μm or less.
[0060] 50. The process of embodiment 49, further comprising: d) optionally annealing the sintered yttrium oxide body by heating the sintered yttrium oxide body to an annealing temperature and performing annealing; e) reducing the temperature of the annealed sintered yttrium oxide body to ambient temperature by removing the heat source applied to the sintered yttrium oxide body; and f) optionally machining the sintered yttrium oxide body to produce a sintered yttrium oxide body component, the component being selected from the group consisting of a dielectric or RF window, a focus ring, a nozzle or gas injector, a showerhead, a gas distribution plate, an etch chamber liner, a plasma source adapter, a gas inlet adapter, a diffuser, an electronic wafer chuck, a chuck, a puck, a mixing manifold, an ion suppressor element, a faceplate, an isolator, a spacer, and a guard ring.
[0061] Embodiment 51. The process of any one of embodiments 49-50, wherein the yttrium oxide powder is calcined prior to step a).
[0062] Embodiment 52. The process of any one of embodiments 49 to 51, wherein the pressure applied to the yttrium oxide during heating is from 10 MPa to 40 MPa.
[0063] Embodiment 53. The process of any one of embodiments 49 to 52, wherein the pressure applied to the yttrium oxide during heating is from 20 MPa to 40 MPa.
[0064] Embodiment 54: The yttrium oxide powder is 1.5 to 7.0 m 2 The process of any one of embodiments 49 to 53, having a surface area of 1 / g.
[0065] Embodiment 55 Yttrium oxide powder is 2.0 to 4.0 m 2 The process of any one of embodiments 49 to 54, having a surface area of 1 / g.
[0066] Embodiment 56. The process of any one of embodiments 49-55, wherein the purity of the yttrium oxide powder is greater than 99.998%.
[0067] Embodiment 57. The process of any one of embodiments 49-56, wherein the purity of the yttrium oxide powder is greater than 99.999%.
[0068] Embodiment 58. The process of any one of embodiments 49 to 57, wherein the sintered yttrium oxide body has a purity of 99.99 to 99.999%.
[0069] Embodiment 59. The process of any one of embodiments 49 to 58, wherein the sintered yttrium oxide body has a purity of 99.999 to 99.9996%.
[0070]
[0046] Embodiment 60. The process of any one of embodiments 49 to 59, wherein sintering is carried out for a time period between 1 minute and 120 minutes.
[0071] Embodiment 61. The process of any one of embodiments 49 to 60, wherein sintering is carried out for a time period between 2 minutes and 60 minutes.
[0072]
[0046] Embodiment 62. The sintered yttrium oxide body has a mass of 4.96 g / cm 3 62. The process of any one of embodiments 49 to 61, having a density equal to or greater than 62.
[0073]
[0046] Embodiment 63: The sintered yttrium oxide body has a mass of 4.98 g / cm 3 63. The process of any one of embodiments 49 to 62, having a density equal to or greater than 63.
[0074]
[0046] Embodiment 64. The sintered yttrium oxide body has a mass of 5.01 g / cm 3 64. The process of any one of embodiments 49 to 63, having a density equal to or greater than 64.
[0075] Embodiment 65. The process of any one of embodiments 49 to 64, wherein any pore on at least one surface has a diameter of 4 μm or less.
[0076] Embodiment 66. The process of any one of embodiments 49 to 65, wherein any pore on at least one surface has a diameter of 3 μm or less.
[0077] Embodiment 67. The process of any one of embodiments 49 to 66, wherein any pore on at least one surface has a diameter of 2 μm or less.
[0078] Embodiment 68. The process of any one of embodiments 49 to 67, wherein any pore on at least one surface has a diameter of 1 μm or less.
[0079] Embodiment 69. The process of any one of embodiments 49-68, wherein the sintered yttrium oxide body has a total impurity level of 35 ppm or less.
[0080] Embodiment 70. The process of any one of embodiments 49-69, wherein the sintered yttrium oxide body has a total impurity level of 30 ppm or less.
[0081] Embodiment 71. The process of any one of embodiments 49-70, wherein the sintered yttrium oxide body has a total impurity level of 25 ppm or less.
[0082] Embodiment 72. The process of any one of embodiments 49-71, wherein the sintered yttrium oxide body has a total impurity level of 20 ppm or less.
[0083] Embodiment 73. The process of any one of embodiments 49-72, wherein the sintered yttrium oxide body has a total impurity level of 15 ppm or less.
[0084] Embodiment 74. The process of any one of embodiments 49-73, wherein the sintered yttrium oxide body has a total impurity level of 10 ppm or less.
[0085] Embodiment 75. The process of any one of embodiments 49-74, wherein the sintered yttrium oxide body has a total impurity level of 6 ppm or less.
[0086]
[0043] Embodiment 76: A sintered yttrium oxide body is etched to a thickness of about 375,000 μm in a process in which a 10 mm×5 mm area of at least one surface is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volt bias, and 2000 watts ICP power. 3 76. The process of any one of embodiments 49-75, wherein the process exhibits an etch volume of less than 100 nm, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm for 1500 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, the first step and the second step being repeated successively until the time of CF4 exposure in the first step is 24 hours.
[0087]
[0046] Embodiment 77: A sintered yttrium oxide body having a diameter of about 325,000 μm 3 77. The process of any one of embodiments 49 to 76, wherein the process exhibits an etch volume of less than 100 nm.
[0088]
[0046] Embodiment 78: A sintered yttrium oxide body having a diameter of about 275,000 μm 3 78. The process of any one of embodiments 49 to 77, wherein the process exhibits an etch volume of less than 100 nm.
[0089] Embodiment 79. The process of any one of embodiments 49-78, wherein the sintered yttrium oxide body has a pore size distribution having a maximum pore size of 1.50 μm for 95% or more of all pores on at least one surface.
[0090] Embodiment 80. The process of any one of embodiments 49 to 79, wherein the sintered yttrium oxide body has a pore size distribution having a maximum pore size of 1.75 μm for 97% or more of all pores on at least one surface.
[0091] Embodiment 81. The process of any one of embodiments 49-80, wherein the sintered yttrium oxide body has a pore size distribution having a maximum pore size of 2.00 μm for 99% or more of all pores on at least one surface.
[0092] Embodiment 82: The process of any one of embodiments 49-81, wherein the sintered yttrium oxide body exhibits an etch rate of less than 1.0 nm / min in a process where a 10 mm×5 mm area of at least one surface is subjected to etching conditions of a pressure of 10 mTorr, an argon flow rate of 20 sccm, a bias of 600 volts, and an ICP power of 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm for 1500 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and the first step and the second step are repeated successively until the time of CF4 exposure in the first step is 24 hours.
[0093] Embodiment 83. The process of any one of embodiments 49 to 82, wherein the etching rate is less than 0.9 nm / min.
[0094] Embodiment 84. The process of any one of embodiments 49 to 83, wherein the etching rate is less than 0.8 nm / min.
[0095]
[0043] In an embodiment 85, the sintered yttrium oxide body has a porosity of 250×10 in the non-etched area, as determined by ISO standard 25178-2-2012, section 4.3.2. -5 The process according to any one of embodiments 49 to 84, wherein the process exhibits a developed interfacial area Sdr of less than 100 μm.
[0096] In the non-etched region of embodiment 86, the developed interface area is 225×10 -5 The process of any one of embodiments 49 to 85, wherein the
[0097] In the non-etched region of embodiment 87, the developed interface area is 200×10 -5 The process of any one of embodiments 49 to 86, wherein the
[0098]
[0043] In a process in which a 6 mm x 6 mm area of at least one surface is subjected to etching conditions of a pressure of 10 mTorr, a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm, an argon flow rate of 20 sccm, and an ICP power of 600 volts and 2000 watts, the sintered yttrium oxide body is etched to a thickness of 200 x 10 Å as determined by ISO standard 25178-2-2012, section 4.3.2. -5 The process of any one of embodiments 49-87, wherein the process exhibits a developed interface area of less than 100 μm.
[0099] In the etched region of embodiment 89, the developed interface area is 175×10 -5 The process of any one of embodiments 49 to 88, wherein the
[0100] In the etched region of embodiment 90, the developed interface area is 150×10 -5 The process of any one of embodiments 49 to 89, wherein the
[0101] Embodiment 91 The process of any one of embodiments 49 to 90, wherein the sintered yttrium oxide body exhibits an arithmetic mean height Sa of less than 30 nm as determined by ISO standard 25178-2-2012, section 4.1.7, in a process in which a 10 mm x 5 mm area of at least one surface is subjected to etching conditions at a pressure of 10 mTorr, an argon flow rate of 20 sccm, and an ICP power of 600 volts and 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm for 300 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and steps 1 and 2 are repeated consecutively for a total etching time of 6 hours.
[0102] The process of any one of embodiments 49 to 91, wherein Sa is less than 20.
[0103] The process of any one of embodiments 49 to 92, wherein Sa is less than 15.
[0104] Embodiment 94. The process of any one of embodiments 49 to 93, wherein at least one surface has an area that is less than 0.15% occupied by pores.
[0105] Embodiment 95. The process of any one of embodiments 49 to 94, wherein at least one surface has an area less than 0.10% occupied by pores.
[0106]
[0046] Embodiment 96: The process of any one of embodiments 49 to 95, wherein the sintered yttrium oxide body has a grain size d50 of 0.1 μm to 25 μm.
[0107] Embodiment 97. The process of any one of embodiments 49 to 96, wherein the sintered yttrium oxide body has a grain size d50 of 0.5 μm to 15 μm.
[0108] Embodiment 98. The process of any one of embodiments 49 to 97, wherein the sintered yttrium oxide body has a grain size d50 of 0.5 μm to 10 μm.
[0109] Embodiment 99. The process of any one of embodiments 49 to 98, wherein the sintered yttrium oxide body has at least one dimension between 100 mm and 600 mm.
[0110]
[0046] Embodiment 100. The process of any one of embodiments 49 to 99, wherein the sintered yttrium oxide body has at least one dimension between 100 mm and 406 mm.
[0111] Embodiment 101. The process of any one of embodiments 49 to 100, wherein the sintered yttrium oxide body has at least one dimension between 200 mm and 600 mm.
[0112] Embodiment 102. The process of any one of embodiments 49 to 101, wherein the sintered yttrium oxide body has at least one dimension between 350 mm and 600 mm.
[0113] Embodiment 103. The process of any one of embodiments 49 to 102, wherein the sintered yttrium oxide body has at least one dimension between 500 mm and 600 mm.
[0114] Embodiment 104. The process of any one of embodiments 49 to 103, wherein the sintered yttrium oxide body has at least one dimension between 550 mm and 600 mm.
[0115] Embodiment 105. The process of any one of embodiments 49-104, wherein the density does not vary by more than 3% along at least one dimension.
[0116] Embodiment 106. The process of any one of embodiments 49-105, wherein the density does not vary by more than 2% along at least one dimension.
[0117] Embodiment 107. The process of any one of embodiments 49-106, wherein the density does not vary by more than 1% along at least one dimension.
[0118] Embodiment 108. The process of any one of embodiments 49 to 107, wherein the sintered yttrium oxide body exhibits a step change of 0.27 to 0.28 μm after the SF6 etching process.
[0119] Embodiment 109. The process of any one of embodiments 49 to 108, wherein the inner wall of the die comprises at least one conductive foil.
[0120]
[0081] Embodiment 110. The process of embodiment 109, wherein at least one conductive foil comprises graphite, niobium, nickel, molybdenum, or platinum.
[0121] Embodiment 111. The process of any one of embodiments 109-110, wherein the die, the upper punch, and the lower punch comprise at least one graphite material.
[0122]
[0081] Embodiment 112. The process of embodiment 111, wherein the at least one graphite material has a particle size selected from the group consisting of 1-50 um, 1-40 um, 1-30 um, 1-20 um, 5-50 um, 5-40 um, 5-30 um, 5-20 um, 5-15 um, and 5-10 um.
[0123] Embodiment 113. The process of any one of embodiments 111-112, wherein the at least one graphite material has a density selected from the group consisting of 1.45-2.0 g / cc, 1.45-1.9 g / cc, 1.45-1.8 g / cc, 1.5-2.0 g / cc, 1.6-2.0 g / cc, 1.7-2.0 g / cc, and 1.7-1.9 g / cc.
[0124]
[0036] Embodiment 114: At least one graphite material has a thermal expansion coefficient of 0.3×10 -6 / ℃ or less, 0.2×10 -6 / ℃ or less, 0.1×10 -6 / ℃ or less, 0.08×10 -6 / ℃ or less, and 0.06×10 -6 114. The process of any one of embodiments 110-113, wherein the temperature varies about the central axis by at least one amount selected from the group consisting of: / °C or less.
[0125] The above-described embodiments of the sintered yttrium oxide body and the process for making the sintered yttrium oxide body may be combined in any manner, and the embodiments may be combined. Thus, the features described above may be combined to describe the yttrium oxide body and / or the process, and vice versa, as outlined in the following description. [Brief description of the drawings]
[0126] These developments are described by way of example with reference to the accompanying drawings, in which features disclosed in relation to the sintered yttrium oxide body also apply to the process and vice versa. [Figure 1] FIG. 1 illustrates a semiconductor processing system in accordance with an embodiment of the present technique. [Diagram 2] FIG. 1 illustrates another embodiment of a semiconductor processing system in accordance with embodiments of the present technique. [Diagram 3] FIG. 1 is a cross-sectional view of an SPS sintering apparatus with a toolset positioned within a vacuum chamber (not shown) with a simple configuration used to sinter ceramic materials. [Figure 4A] FIG. 4 shows the embodiment of FIG. 3 showing one foil layer. [Figure 4B] FIG. 4 illustrates an alternative embodiment of FIG. 3 showing two foil layers. [Figure 4C] FIG. 4 illustrates another alternative embodiment of FIG. 3 showing three foil layers. [Figure 5A] FIG. 4 is a top view of the SPS sintering apparatus of FIG. 3. [Figure 5B] FIG. 4 is a top view of the SPS sintering apparatus of FIG. 3. [Figure 6] 1 is a graph showing the radial variation of the average coefficient of thermal expansion (CTE) of graphite materials A and B at 1200° C. [Figure 7] Figure 7a shows the standard deviation (ppm) of the thermal expansion coefficients of graphite materials A and B. Figure 7b shows the dispersion of the thermal expansion coefficients of graphite materials A and B, respectively, measured over the operating temperature range of 200 to 1200°C. [Figure 8] 1 is a graph showing the thermal expansion coefficients of graphite materials A and B at 400 to 1400° C. [Figure 9] EDS (energy dispersive X-ray spectroscopy) spectra obtained from selected areas on the grain boundaries. [Figure 10]FIG. 13 shows the results of over-coverage in atoms / nm2 across several grain boundaries of example sample 107. [Figure 11] FIG. 13 shows the results of over-coverage in atoms / nm2 across several grain boundaries of example sample 114. [Figure 12] FIG. 1 shows the CF etch volume of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 compared to sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 according to embodiments of the present disclosure after a single-step CF etching process as disclosed herein. [Figure 13] FIG. 1 shows the CF4+O2 average etch volume (after the two-step etching process disclosed herein) of prior art TSC 03 (quartz) and sintered yttrium oxide samples 118 and 107 compared to various sintered yttrium oxide samples made according to embodiments of the present disclosure. [Figure 14] FIG. 1 shows the CF4+O2 average step height (after a two-step etching process) of prior art TSC 03 (quartz) and sintered yttrium oxide samples 118 and 107 compared to various sintered yttrium oxide samples made according to embodiments of the present disclosure. [Figure 15] FIG. 1 shows the CF4+O2 average etch rate (after a two-step etch process) of prior art TSC 03 (quartz), sintered yttrium oxide samples 118 and 107 compared to various samples made according to embodiments of the present disclosure. [Figure 16] FIG. 1 shows 50x SEM micrographs of the surfaces of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 before and after a single-step CF4 etching process. [Figure 17] FIG. 13 shows 50x SEM micrographs of the surfaces of sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 made in accordance with the present disclosure before and after a single-step CF4 etching process. [Figure 18] FIG. 1 shows 1000X SEM micrographs of the surfaces of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 before and after a single-step CF4 etching process. [Figure 19] FIG. 1000X SEM micrographs of the surfaces of sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 made in accordance with the present disclosure before and after a single-step CF4 etching process. [Figure 20] FIG. 1 shows 5000x SEM micrographs of the surfaces of prior art sintered yttrium oxide samples 107 and 118 before and after the single-step CF4+O2 etching process. [Figure 21] FIG. 13 shows SEM micrographs at 5000x of the surfaces of sintered yttrium oxide samples 152 and 189-1 made according to the present disclosure before and after a two-step CF4 + O2 etching process. [Figure 22] 1 shows SEM micrographs at 1000× and 5000× of the edge surface of a sintered yttrium oxide sample made according to the present disclosure and the center surface of the same sintered yttrium oxide sample 457. [Diagram 23] FIG. 2 shows that yttrium oxide bodies (H1 / 66 to H4 / 152) according to one embodiment of the present disclosure do not have pores with a pore size greater than 2.00 μm. [Figure 24] 1 is a graph showing the developed interfacial area ratio Sdr at 50x optical magnification for prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 compared to sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 according to embodiments of the present disclosure before and after a single-step CF4 etching process. [Diagram 25] 1 is a graph showing the arithmetic mean height Sa (nm) measured at 50x optical magnification of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 compared to sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 according to embodiments of the present disclosure before and after a single-step CF4 etching process. [Figure 26] 1 is a graph showing the developed interfacial area ratio Sdr measured at 50x optical magnification of prior art sintered yttrium oxide sample CM1 / 107 and various sintered yttrium oxide samples from the examples before and after a two-step CF4+O2 etching process. [Figure 27] FIG. 1 is a graph showing the arithmetic mean height Sa (nm) measured at 50× optical magnification of prior art sintered yttrium oxide sample CM1 / 107 and various samples from the examples before and after a two-step CF4+O2 etching process. [Figure 28] 1 is a graph showing the areal porosity of various sintered yttrium oxide samples from the examples compared to prior art sintered yttrium oxide samples. [Figure 29] 1 is a graph showing cumulative area (%) versus pore size (pore size distribution) for various samples from the examples compared to a prior art sintered yttrium oxide sample. [Diagram 30] 1 is a graph showing porosity distribution versus log pore size for various samples from the examples compared to prior art sintered yttrium oxide samples. [Diagram 31] 1 is a graph showing the sintering pressure and temperature conditions required to obtain a sintered yttrium oxide body having a density of 98% or greater relative to the theoretical density of yttrium oxide. [Diagram 32] 1 is a flow chart of the quantification procedure of the Zeta factor method with X-ray absorption correction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0127] Sintered yttrium oxide bodies are proposed as materials for parts used in plasma etch processing chambers prepared by the sintering process disclosed herein. Such parts may include, among other components, windows, nozzles, showerheads, (etch) chamber liners, mixing manifolds, wafer supports, electronic wafer chucks, and various rings such as focus rings and guard rings.
[0128] Reference will now be made in detail to certain embodiments. Examples of specific embodiments are illustrated in the accompanying drawings. Although the present disclosure will be described in conjunction with these specific implementations, it will be understood that it is not intended to limit the present disclosure to such specific embodiments. On the contrary, it is intended to cover alternatives, modifications, and equivalents that may be included within the spirit and scope as defined by the appended claims. In the following description, numerous specific details are set forth in order to provide a thorough understanding of the disclosed embodiments. The present disclosure may be practiced without some or all of these specific details.
[0129] definition As used herein, the terms "semiconductor wafer," "wafer," "substrate," and "wafer substrate" are used interchangeably. Wafers or substrates used in the semiconductor device industry typically have diameters of, for example, 200 mm, or 300 mm, or 450 mm.
[0130] As used herein, the term "sintered yttrium oxide body" is synonymous with "sinter," "body" or "sintered body" or "ceramic sintered body" and refers to a solid article that comprises yttrium oxide and is formed when subjected to a pressure and heat treatment process that produces a monolithic sintered yttrium oxide body from a yttrium oxide powder as disclosed herein.
[0131] As used herein, the term "purity" refers to the presence of various contaminants that are typically considered deleterious in an application in the starting material from which a sintered yttrium oxide body may be formed, as disclosed herein.
[0132] As used herein, the term "impurities" refers to elements, compounds, or other substances present in the starting materials or processes from which the sintered yttrium oxide body may be formed, and which are typically considered deleterious in applications. The impurity content is measured relative to the total mass of the yttria powder or sintered yttria body.
[0133] As used herein, the term "tool set" can include a die and upper and lower punches.
[0134] As used herein, the terms "stiffness" and "rigidity" are synonymous and are consistent with the definition of Young's modulus, as known to those skilled in the art.
[0135] The terms "calcination" or "calcining", when used in reference to a heat treatment process, are understood herein to mean a heat treatment step that can be performed on a powder in air at a temperature below the sintering temperature to remove moisture and / or impurities, increase crystallinity, and potentially modify the powder mixture surface area.
[0136] The term "annealing", as applied to ceramic heat treatment, is understood herein to mean a heat treatment performed in air on the disclosed sintered yttrium oxide bodies to a temperature and slowly cooled to relieve stress and / or normalize stoichiometry.
[0137] The term "Sa" as known in the art refers to the arithmetic mean height of a surface and represents the absolute value of the arithmetic mean over the surface. The definition according to ISO 25178-2-2012 section 4.1.7 is the arithmetic mean of the absolute values of the ordinate values within a defined area (A).
[0138] The term "Sdr", as known in the art, refers to a calculated numerical value defined as the "Developed Interfacial Area Ratio", which is a proportional expression for the increase in actual surface area over the surface area of a perfectly flat surface. The definition according to ISO 25178-2-2012 section 4.3.2 is the ratio of the increment in interfacial area of the scale-limiting surface within a defined area (A) to the defined area.
[0139] As used herein, the term "about" when used in connection with a number permits a variation of plus or minus 10%.
[0140] In the following description, a given range includes a lower threshold and an upper threshold. Thus, a definition of a parameter A in the sense of "within the range of X and Y" or "within the range of X to Y" means that A can be any value of X, Y and any value from X to Y. A definition of a parameter A in the sense of "up to Y" or "at least X" therefore means that A can be any value less than Y and Y, or A can be any value greater than X and X, respectively.
[0141] Sintered yttrium oxide body The following detailed description assumes that the invention is implemented in an apparatus such as an etch chamber or deposition chamber required as part of the manufacture of semiconductor wafer substrates. However, the invention is not so limited. The workpieces may be of various shapes, sizes, and materials. In addition to semiconductor wafer processing, other workpieces that may utilize the invention include various articles such as inorganic circuit boards with fine feature sizes, magnetic recording media, magnetic recording sensors, mirrors, optical elements, micromechanical devices, and the like.
[0142] Semiconductor processing reactors associated with etch or deposition processes require chamber components fabricated from materials that are highly resistant to chemical attack by the reactive plasmas required for semiconductor processing. These plasmas or process gases can be a variety of halogen, oxygen, and nitrogen based chemicals, such as O2, F, Cl2, HBr, BCl3, CCl4, and HCl. 4、 N 2、 NF3, NO, NO, C2H 4、 CF4, SF6, C4F8, CHF 3、 The use of the corrosion resistant materials disclosed herein results in reduced chemical corrosion during use.
[0143] 1 and 2 show an etch / deposition chamber in which the sintered yttrium oxide bodies disclosed herein are useful. As shown in FIG. 1, an embodiment of the present technology can include a semiconductor processing system 9500, also referred to as a processing system. The processing system 9500 can include a remote plasma region. The remote plasma region can include a plasma source 9502, also referred to as a remote plasma source ("RPS").
[0144] The processing system 9500, which may represent a capacitively coupled plasma (CCP) processing apparatus, includes a vacuum chamber 9550, a vacuum source, and a chuck 9508 on which a wafer 50, also called a semiconductor substrate, is supported. A window 9507 forms the upper wall of the vacuum chamber 9550. The window 9507 may be made of a sintered yttrium oxide body according to one of the previously described embodiments. In some embodiments, the window 9507 may be partially made of a sintered yttrium oxide body according to one of the previously described embodiments. 9506 may be a gas inlet, gas inlet assembly gas delivery system, injector or nozzle, which may be made of a sintered yttrium oxide body. The gas injector 9506 may comprise a separate member of the same or different material as the window.
[0145] The plasma source 9502 is provided outside a window 9507 of a vacuum chamber 9550 for accommodating a wafer 50 to be processed. In the vacuum chamber 9550, a capacitively coupled plasma can be generated by supplying a processing gas to the vacuum chamber 9550 and supplying a high frequency power to the plasma source 9502. A predetermined plasma processing is performed on the wafer 50 using the capacitively coupled plasma thus generated. A planar antenna having a predetermined pattern is widely used as a high frequency antenna for the capacitively coupled processing system 9500.
[0146] The processing system 9500 may further include an electrostatic chuck 9508 designed to support the wafer 50. The chuck 9508 may include a puck 9509 for supporting the wafer 50. The puck 9509 may have a chucking electrode disposed within the puck proximate a support surface of the puck 9509 for electrostatically holding the wafer 50 when placed on the puck 9509. The chuck 9508 may include a ring-shaped base 9511 extending to support the puck 9509, and a shaft 9510 disposed between the base and the puck and supporting the puck above the base such that a space is formed between the puck 9509 and the base 9510, the shaft 9510 supporting the puck proximate a periphery of the puck 9509. The puck 9509 may be made of a sintered yttrium oxide body according to one of the previous embodiments to minimize generated particles that may contaminate the wafer.
[0147] In a physical vapor deposition (PVD) process, a substrate ring including a cover ring 9514 is provided around the substrate. The cover ring 9514 typically has a lip or ledge that surrounds the wafer and rests on the wafer support surface of the puck 9509. The cover ring 9514 shields the sidewall surfaces and periphery of the puck 9509 from deposition of process residues that would otherwise be exposed to the excited gases in the chamber. Thus, the cover ring 9514 reduces the buildup of process residues on the puck 9509. Such buildup of process residues will eventually flake off and contaminate the wafer. The cover ring 9514 may be made of a sintered yttrium oxide body according to one of the embodiments described above.
[0148] The cover ring 9514 can reduce erosion of the puck 9509 by the excitation gas. Providing the cover ring 9514 also reduces the frequency with which the chuck and / or puck 9509 require cleaning, since the cover ring itself can be periodically removed from the chamber and cleaned, for example with HF and HNO3, to remove processing residues that build up on the ring during substrate processing cycles. The arrangement of the cover ring 9514 can be seen in FIG. 1, where the cover ring covers a portion of the support surface of the puck 9509. Further portions of the surface of the puck 9509 may be covered by the upper shield ring 9512 and / or shield ring 9513. To have a suitably high erosion and corrosion resistance, the upper shield ring 9512 and / or shield ring 9513 may be made of a sintered yttrium oxide body according to one of the embodiments described above.
[0149] As shown in FIG. 2, another embodiment of the present technology can include a semiconductor processing system 9600. The processing system 9600, which can represent an inductively coupled plasma (ICP) processing apparatus, includes a vacuum chamber 9650, a vacuum source, and a chuck 9608 on which a wafer 50, also referred to as a semiconductor substrate, is supported. A showerhead 9700 forms an upper wall of the vacuum chamber 9650 or is attached below the upper wall. The ceramic showerhead 9700 includes a gas plenum in fluid communication with a plurality of showerhead gas outlets for supplying process gas to the interior of the vacuum chamber 9650. Furthermore, the showerhead 9700 can include a central opening configured to receive a central gas injector. An RF energy source excites the process gas into a plasma state to process the semiconductor substrate. The flow rate of the process gas provided by the central gas injector and the flow rate of the process gas provided by the ceramic showerhead 9700 can be independently controlled. The processing system 9600 can include a showerhead 9700, which can be made of a sintered yttrium oxide body according to one of the previous embodiments. The showerhead 9700 can be in fluid communication with a gas delivery system 9606. The gas delivery system 9606 can be made from a sintered yttrium oxide body and can have an injector or nozzle 9714 made from a sintered yttrium oxide body.
[0150] The system 9600 may further include a chuck 9608 designed to support the wafer 50. The chuck 9608 may include a puck 9609 for supporting the wafer 50. The puck 9609 may be formed from a dielectric material and may have a chucking electrode disposed within the puck proximate a support surface of the puck 9609 for electrostatically holding the wafer 50 when placed on the puck 9609. The chuck 9608 may include a ring-shaped base 9611 extending to support the puck 9609, and a shaft 9610 disposed between the base and the puck and supporting the puck above the base such that a space is formed between the puck 9609 and the base 9610, the shaft 9610 supporting the puck proximate a periphery of the puck 9609. The puck 9609 may be made of a sintered yttrium oxide body according to one of the previous embodiments to minimize generated particles that may contaminate the wafer.
[0151] A portion of the surface of the showerhead 9700 may be covered with a shield ring 9712. A portion of the surface of the showerhead 9700, in particular a radial side of the surface of the showerhead 9700, may be covered with an upper shield ring 9710. A portion of the support surface of the puck 9609 may be covered with a cover ring 9614. Further portions of the surface of the puck 9609 may be covered with an upper shield ring 9612 and / or an insulator ring 9613. To have suitably high erosion and corrosion resistance, the cover ring 9614 and / or the upper shield ring 9612 and / or the insulator ring 9613 may be made from a sintered yttrium oxide body according to one of the previous embodiments.
[0152] The showerhead 9700 may include two parallel plates, both of which may include or consist of a sintered yttrium oxide body according to one of the embodiments disclosed herein. The two plates may be bonded together to define a volume between the plates. The bonding of the plates may be made to provide a fluid channel through the upper plate and the lower plate. The showerhead may distribute process gases through the fluid channel, including upon excitation by a plasma in the chamber plasma region or plasma effluent from the plasma source. An ion suppressor (not shown) may be disposed proximate to a surface of the second plate and may be bonded to a surface of the second plate. The ion suppressor may include or consist of a sintered yttrium oxide body according to one of the embodiments disclosed herein. The ion suppressor may be configured to reduce ion migration to a processing region of a processing chamber housing a wafer. The ion suppressor may define a number of openings through the structure.
[0153] The sintered yttrium oxide bodies disclosed herein can be useful as sintered ceramic components in plasma processing chambers designed for either semiconductor etching and / or deposition processes.
[0154] For example, providing a chamber component material such as a sintered yttria ceramic body with very high purity provides a uniform corrosion resistant body with few impurities that can act as sites for initiation of corrosion. High resistance to erosion or spalling is also required for materials for use as chamber components. However, as discussed above, erosion can result from ion bombardment of the component surface from the use of inert plasma gases such as Ar. Furthermore, components fabricated from dense materials with minimal porosity distributed on a fine scale can provide greater resistance to corrosion and erosion during etching and deposition processes. As a result, preferred chamber components may be fabricated from materials that have high erosion and corrosion resistance during plasma etching, deposition and chamber cleaning processes. This resistance to corrosion and erosion prevents the release of particles from the component surface into the etching or deposition chamber during semiconductor processing. Such particle release or emission into the process chamber contributes to wafer contamination, semiconductor process drift, and semiconductor device level yield loss.
[0155] In addition, chamber components must possess sufficient bending strength and stiffness for the handling required during component installation, removal, cleaning, and use within the process chamber. High mechanical strength allows intricate features of fine geometry to be machined into the sintered ceramic without breakage, cracking, or chipping. Bending strength or stiffness becomes especially important with the large component sizes used in modern process tools. Some component applications, such as chamber windows on the order of 200-600 mm in diameter, subject the windows to significant stresses during use under vacuum conditions, necessitating the selection of corrosion-resistant materials of high strength and stiffness.
[0156] The ceramic sintered bodies and related components disclosed herein provide improved plasma etch resistance and enhanced ability to be cleaned in semiconductor processing chambers due to certain material properties and characteristics described below.
[0157] Total impurity level below 40ppm, 4.93g / cm 3 Disclosed herein is a sintered yttrium oxide body having a density of at least 5 μm, the sintered yttrium oxide body having at least one surface that includes at least one pore, each pore having a diameter of 5 μm or less. The sintered yttrium oxide body disclosed herein is provided by applying a specific preparation procedure and certain specific process parameters in a spark plasma sintering (SPS) process, as described in more detail herein below.
[0158] The sintered yttrium oxide body produced by the methods disclosed herein has a total impurity level of 40 ppm or less. In one embodiment, the sintered yttrium oxide body has a total impurity level of 35 ppm or less. In another embodiment, the sintered yttrium oxide body has a total impurity level of 30 ppm or less. In another embodiment, the sintered yttrium oxide body has a total impurity level of 25 ppm or less. In yet another embodiment, the sintered yttrium oxide body has a total impurity level of 20 ppm or less. In yet another embodiment, the sintered yttrium oxide body has a total impurity level of 15 ppm or less. In yet another embodiment, the sintered yttrium oxide body has a total impurity level of 10 ppm or less. In yet another embodiment, the sintered yttrium oxide body has a total impurity level of 5 ppm or less. In yet another embodiment, the sintered yttrium oxide body has a total impurity level of 0 ppm. As used herein, the term "impurities" refers to any element or compound other than yttrium oxide. Exemplary impurities include, but are not limited to, silicon, calcium, sodium, strontium, zirconia, magnesium, potassium, iron, phosphorus, boron, and low melting point elements such as zinc, tin, and indium. Thus, in embodiments, the sintered yttrium oxide body is substantially free or free of at least one or all of these impurities.
[0159] The sintered yttrium oxide body of the present disclosure has a density of 4.93 g / cm, which is 98% of theoretical density. 3 DRLide, CRC Handbook of Chemistry and Physics 84 th According to the CRC Handbook, Edition, 2012, the theoretical density of yttrium oxide is 5.03 g / cm 3 Sintered yttrium oxide bodies made according to the present disclosure have a density of 98% or more, preferably 98.5% or more, more preferably 99% or more, even more preferably 99.5% or more, and even more preferably 100% or more of the theoretical density of yttrium oxide as set forth in the CRC Handbook. That is, the sintered yttrium oxide bodies disclosed herein have a density of 4.93 g / cm 3 or greater (98% or greater of theoretical). In some embodiments, the sintered yttrium oxide bodies disclosed herein have a density of 4.96 g / cm 3 In other embodiments, the sintered yttrium oxide bodies disclosed herein have a density of 4.98 g / cm or more (98.5% or more of theoretical). 3 In yet another embodiment, the sintered yttrium oxide body disclosed herein has a density of 5.01 g / cm or more (density of 99% or more of theoretical value). 3 The density is 99.5% or more of the theoretical value. The deviation of the density measurement is measured and is less than 0.002 g / cm 3and thus measurements may vary accordingly. Density measurements were performed using the Archimedes method known to those skilled in the art. Thus, the sintered yttrium oxide bodies disclosed herein do not include mixtures of yttrium oxide with other oxides, such as, for example, zirconium oxide or aluminum oxide, but rather, the sintered yttrium oxide bodies disclosed herein consist essentially of or consist of yttrium oxide consistent with the potential impurity levels described above. Prior art solutions require combining yttrium oxide with other materials to increase the bending strength required for application in large-scale semiconductor processing systems. The disclosed process and material combinations provide high purity sintered bodies with greater than 98% theoretical density. Successful production of sintered yttrium oxide bodies across the longest dimension (approximately greater than 200 mm to 600 mm) may also be enabled by controlling the variation in density across at least one longest dimension. Densities less than 98% may also result in greater density variation and reduced strength and handleability, therefore a density of at least 98% is desirable, with a density variation of less than 3% across at least one dimension, which may be the longest dimension. The disclosed solid yttrium oxide bodies were tested using a four-point bend technique in accordance with ASTM C1161-13 and measured an average bend strength of 224 MPa with a standard deviation of 14 MPa.
[0160] Mechanical strength properties are known to improve with decreasing grain size. To evaluate grain size, linear intercept grain size measurements were performed according to the Heyn Linear Intercept Procedure described in ASTM standard E112-2010 "Standard Test Method for Determining Average Grain Size". Grain size measurements were also performed using Electron Backscatter Diffraction (EBSD) techniques known in the art. To meet the high bending strength and stiffness requirements for use in reaction chambers as large components of 100-600 mm, the ceramic sintered body may have a fine grain size, for example, a grain size d50 of 0.1 μm to 25 μm, in some embodiments 1 μm to 20 μm, in other embodiments 0.5 μm to 20 μm, in other embodiments 0.5 μm to 15 μm, in still other embodiments 0.5 μm to 10 μm, in other embodiments 0.75 to 5 um, in other embodiments 2 μm or less, in other embodiments 1.5 μm or less, and in still other embodiments 1.0 μm or less. These grain sizes can result in a sintered yttrium oxide body having a four-point bending strength according to ASTM C1161-13 of 250 MPa or less, 300 MPa or less, preferably 350 MPa or less, preferably at least 400 MPa or less. Too large a grain size in diameter, on the order of more than 25 um, can result in a sintered body with low bending strength values that may make it unsuitable for use as an etching and / or deposition chamber component, particularly of large dimensions, and therefore the sintered yttrium oxide body preferably has an average grain size of less than 13 um (i.e., 0.01 μm to 13 μm).
[0161] The sintered yttrium oxide bodies disclosed herein have very small pores both on the surface and throughout the body. Preferably, the sintered yttrium oxide body made according to the processes disclosed herein is therefore a monolithic body with pores throughout the body. In other words, the porous structure measured on the surface can represent the porosity level within the bulk yttrium oxide body, as detailed in more detail below.
[0162] The sintered yttrium oxide bodies disclosed herein have at least one surface comprising at least one pore, each pore having a diameter of 5 μm or less. In one embodiment, each pore has a diameter of 4.0 μm or less. In one embodiment, each pore has a diameter of 3 μm or less. In another embodiment, each pore has a diameter of 2 μm or less. In yet another embodiment, each pore has a diameter of 1.5 μm or less. In yet another embodiment, each pore has a diameter of 1 μm or less. Pore size can be measured, for example, by scanning electron microscopy (SEM).
[0163] The yttrium oxide body is further characterized by having a pore size distribution with a maximum pore diameter of 1.50 μm for 95% or more of the total pores on at least one surface of the sintered yttrium oxide body, preferably a maximum pore diameter of 1.75 μm for 97% or more, and more preferably a maximum pore diameter of 2.00 μm for 99% or more of the total pores on at least one surface of the sintered yttrium oxide body. The pore size distribution and overall porosity were determined by porosity measurements over an area of the polished sample measuring 5 mm×5 mm using SEM images obtained from a Phenom XL scanning electron microscope. Representative SEM images were taken from the left, right, top and bottom areas of the sample to gather information regarding material uniformity over the entire sample area. Four images at 1000× with image dimensions of 269 um×269 um and four images at 5000× with image dimensions of 53.7 um×53.7 um were analyzed to determine the number of pores, fractional area of porosity and pore diameter over the entire image measurement area. The total image measurement area over which porosity was measured was 0.301 mm 2 For porosity analysis using contrast techniques, the images were imported into ImageJ software. ImageJ, developed at the National Institutes of Health (NIH), is a Java-based public domain image processing and analysis program for image processing of scientific multidimensional images.
[0164] Preferably, the at least one pore occupies less than 0.2%, more preferably less than 0.15%, and most preferably less than 0.1% of the surface area of at least one surface of the sintered yttrium oxide body as determined by the methods disclosed herein.
[0165] Sintered yttrium oxide bodies prepared according to the present development preferably exhibit a step height of 0.2-0.98 μm for the two-step CF4 / O2 etching process disclosed herein, 0.27-0.28 μm for the SF6 etching process disclosed herein, and 0.1-0.13 μm for the O2 etching process disclosed herein. The step height as a result of the etching process can be measured directly by using a Keyence 3D Laser Scanning Confocal Digital Microscope Model VK-X250X at 20x magnification. Selected areas in the etched and unetched regions of the sample are used to create separate reference planes. The average height difference between these reference planes over three measurements is taken as the step height.
[0166] The sintered yttrium oxide bodies disclosed herein have a diameter of about 375,000 μm 3 Less than about 325,000 μm 3 less than about 275,000 μm 3 less than about 175,000 μm 3 The calculated CF4 / O2 etch volume is shown below.
[0167] The disclosed etch volume, etch rate, and step height are measured according to a two-step etching process, the process being carried out on a 10 mm×5 mm area of at least one surface subjected to etching conditions at a pressure of 10 mTorr, an argon flow rate of 20 sccm, a bias of 600 volts, and an ICP power of 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm and an oxygen flow rate of 30 sccm for 1500 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and the first and second steps being repeated consecutively until the time of CF4 exposure in the first step reaches 24 hours. The etch volume as a result of the etching process can be calculated by using a Keyence 3D Laser Scanning Confocal Digital Microscope Model VK-X250X at a magnification of 20 times. The selected area defined in the etched region of the specimen is compared to a reference plane height, and the volume defined by the selected area between the reference plane height and the etched surface is the calculated etch volume, whereby the calculated etch volume is related to the volume of the yttrium oxide body removed during the etching process.
[0168] The sintered yttrium oxide bodies disclosed herein exhibit a calculated etch rate of less than about 1.0 nm / min, preferably less than about 0.90 nm / min, more preferably less than about 0.8 nm / min, more preferably less than about 0.7 nm / min, more preferably less than about 0.6 nm / min, more preferably less than about 0.5 nm / min, more preferably less than about 0.4 nm / min, and more preferably less than about 0.3 nm / min. The etch rate is measured when a two-step etch process is performed, where a 10 mm x 5 mm area of at least one surface is subjected to etch conditions at a pressure of 10 mTorr, an argon flow rate of 20 sccm, a bias of 600 volts, and an ICP power of 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm for 1500 seconds, the second step having a CF4 flow rate of 0 sccm, and an oxygen flow rate of 100 sccm for 300 seconds, the first step and the second step being repeated successively until the time of CF4 exposure in the first step is 24 hours. The etch rate is calculated from the measured step height and the etch time. The etch rate is thereby related to the thickness reduction of the yttrium oxide body removed during the indicated etch process.
[0169] The sintered yttrium oxide body disclosed herein has a porosity of 250×10 in the unetched areas according to ISO standard 25178-2-2012, section 4.3.2. -5 Less than 225×10 -5 Less than 200×10 -5 The surface is typically polished prior to determining the developed interfacial area ratio in the non-etched regions.
[0170] The sintered yttrium oxide body disclosed herein has a porosity of 1500×10 in the etched area according to ISO standard 25178-2-2012, section 4.3.2. -5 Less than 1300×10 -5 Less than 1000×10 -5less than 800×10 -5 Less than 600×10 -5 The developed interface area ratio is further characterized as being less than 10 mm×5 mm, which is determined by a two-step etching process in which at least one surface area of 10 mm×5 mm is subjected to etching conditions of 10 mTorr pressure, 20 sccm argon flow rate, and 600 volts bias and 2000 watts ICP power, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm for 300 seconds, and the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and steps 1 and 2 are repeated consecutively for a total etching time of 6 hours.
[0171] The sintered yttrium oxide body disclosed herein has a porosity of 250×10 in the unetched areas according to ISO standard 25178-2-2012, section 4.3.2. -5 Less than 225×10 -5 Less than 200×10 -5 and in the etched area, have a developed interface area ratio Sdr of less than 1500 × 10 in accordance with ISO standard 25178-2-2012, section 4.3.2. -5 Less than 1300×10 -5 Less than 1000×10 -5 less than 800×10 -5 Less than 600×10 -5This latter developed interface area ratio was determined by a two-step etch process in which a 10 mm×5 mm area of at least one surface was subjected to etch conditions of 10 mTorr pressure, 20 sccm argon flow rate, 600 volts bias and 2000 watts ICP power, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm for 300 seconds, and the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, with steps 1 and 2 being repeated consecutively for a total etch time of 6 hours.
[0172] The sintered yttrium oxide bodies disclosed herein are further characterized in that in the unetched regions, they have an arithmetic mean height Sa of less than 10 nm, more preferably less than 8 nm, and most preferably less than 5 nm, according to ISO standard 25178-2-2012, section 4.1.7. Typically, the surface is polished prior to determining the arithmetic mean height of the unetched regions.
[0173] The sintered yttrium oxide bodies disclosed herein are further characterized as exhibiting an arithmetic mean height Sa of less than 20 nm, more preferably less than 16 nm, and most preferably less than 12 nm, in accordance with ISO Standard 25178-2-2012, Section 4.1.7, determined after a two-step etching process in which a 10 mm×5 mm area of at least one surface is subjected to etching conditions at a pressure of 10 mTorr, an argon flow rate of 20 sccm, and an ICP power of 600 volts and 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm for 300 seconds, the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, and steps 1 and 2 being repeated consecutively for a total etching time of 6 hours.
[0174] In another embodiment, the sintered yttrium oxide body exhibits an arithmetic mean height Sa of less than 10 nm, more preferably less than 8 nm, and most preferably less than 5 nm, according to ISO Standard 25178-2-2012, Section 4.1.7, and an arithmetic mean height Sa of less than 20 nm, more preferably less than 16 nm, and most preferably less than 12 nm, according to ISO Standard 25178-2-2012, Section 4.1.7. The latter arithmetic mean height Sa was achieved when a sample of a sintered yttrium oxide body having an area of 10 mm x 5 mm of at least one surface was subjected to a two-step etching condition at a pressure of 10 mTorr, an argon flow rate of 20 sccm, and a bias of 600 volts and an ICP power of 2000 watts, the process having a first step and a second step, the first step having a CF4 flow rate of 90 sccm, an oxygen flow rate of 30 sccm for 300 seconds, and the second step having a CF4 flow rate of 0 sccm and an oxygen flow rate of 100 sccm for 300 seconds, with steps 1 and 2 being repeated consecutively for a total etching time of 6 hours.
[0175] The above-mentioned sintered yttrium oxide bodies show improved behavior in etching processes and can be easily used as materials for the preparation of etching chamber components. Yttrium oxide materials, typically coatings made from yttrium oxide, have been used in etching chamber components to date and, as already mentioned above, suffer from the main problem of the generation of particles under harsh etching conditions that contaminate the products being processed. The focus of the prior art to avoid such contamination and thus the generation of particles under etching conditions is mainly on the bulk (percentage) porous properties of the yttrium oxide materials used. The challenge of sintering solid yttrium oxide to a sufficiently high density results in a material with lower strength that is not suitable for semiconductor processing chambers requiring components with large dimensions, such as more than 100 mm.
[0176] The sintered yttrium oxide bodies disclosed herein have low dielectric loss due at least in part to the high purity of the sintered bodies listed in Table 9. Dielectric loss may also be affected by grain size and grain size distribution. Finer grain size may also result in reduced dielectric loss, thereby providing reduced heating during use at higher frequencies. Table 13 lists grain sizes for exemplary sintered yttria bodies disclosed herein. 1×10 -4 ~5×10 -2 , preferably 1 x 10 -4 ~1×10 -2 , preferably 1.0 x 10 -2 ~5×10 -2 , preferably 1.5 x 10 -2 ~5.0×10 -2 , more preferably 1×10 -4 ~1×10 -3 can be achieved for sintered ceramic bodies containing high purity fine grained yttrium oxide.
[0177] According to the above features, the microstructure and surface of the resulting sintered yttrium oxide body after etching is uniform and less volume of material is etched while maintaining a low developed surface area, thereby improving the product life cycle and low particle generation characteristics in etching applications.
[0178] The sintered yttrium oxide body disclosed herein is the result of a specific preparation process. Whether the sintered yttrium oxide body exhibits the above-mentioned properties can be easily determined by a person skilled in the art by applying the measurement methods disclosed herein, which at least in part correspond to standard procedures (ISO standards). Thus, a person skilled in the art can directly and reliably verify whether a yttrium oxide material meets the claimed characteristics by tests or procedures appropriately described herein or known to a person skilled in the art. Making these measurements does not require undue experimentation for a person skilled in the art. This process is now disclosed in detail.
[0179] Equipment / Spark Plasma Sintering Tools Disclosed herein is a spark plasma sintering (SPS) tool, comprising: a die including a sidewall including an inner wall and an outer wall, the inner wall having a diameter defining an interior volume capable of receiving at least one ceramic powder; an upper punch and a lower punch operatively coupled to the die, each of the upper punch and the lower punch having an outer wall defining a diameter smaller than the diameter of the inner wall of the die, thereby creating a gap between each of the upper punch and the lower punch and the inner wall of the die as at least one of the upper punch and the lower punch moves within the interior volume of the die, the gap being between 10 μm and 100 μm wide, and in some embodiments between 10 μm and 70 μm wide; and the yttrium oxide powder is between 1 and 10 μm thick as measured according to ASTM C1274. 2 / g specific surface area (SSA).
[0180] FIG. 3 shows an SPS tool 1 with a simplified die / punch arrangement used to sinter ceramic powder. Typically, the die / punch arrangement is within a vacuum chamber (not shown), as will be appreciated by those skilled in the art. With reference to FIG. 3, the spark plasma sintering tool 1 includes a die system 2 including a sidewall that includes an inner wall 8 having a diameter that defines an interior volume capable of receiving yttrium oxide powder 5.
[0181] With further reference to FIG. 3 , the spark plasma sintering tool 1 includes an upper punch 4 and a lower punch 4' operably coupled to the die system 2, the upper punch 4 and the lower punch 4' having an outer wall 11 and defining a diameter smaller than a diameter of an inner wall 8 of the die system 2, thereby creating a gap 3 between each of the upper punch 4 and the lower punch 4' and the inner wall 8 of the die system 2 when at least one of the upper punch 4 and the lower punch 4' is moved within the internal volume of the die system 2.
[0182] The die system 2 and the upper punch 4 and the lower punch 4' may include at least one graphite material. In certain embodiments, the graphite material(s) disclosed herein may include at least one isotropic graphite material. In other embodiments, the graphite material(s) disclosed herein may include at least one reinforced graphite material, such as a carbon-carbon composite, and a graphite material including fibers, particles, or sheets, or meshes, or laminates of other conductive materials, such as carbon, in a matrix of an isotropic graphite material. In other embodiments, the die and the upper and lower punches may include a combination of these isotropic and reinforced graphite materials.
[0183] For example, the graphite material used in some or all of the tool portions, such as the die 6 and the punches 4 and 4', may comprise a porous graphite material exhibiting a porosity of about 5% to about 20%, about 5% to about 17%, about 5% to about 13%, about 5% to about 10%, 5% to about 8%, about 8% to about 20%, about 12% to 20%, about 15% to about 20%, about 11% to about 20%, about 5% to 15%, 6% to about 13%, and preferably about 7% to about 12%.
[0184] Preferably, the graphite material has an average pore size (pore diameter) of 0.4 to 5.0 μm, preferably 1.0 to 4.0 μm, and contains pores with a surface pore diameter of 30 μm or less, preferably 20 μm or less, preferably 10 μm or less. More preferably, pores with a surface pore diameter of 10 to 30 μm may be present.
[0185] The graphite material used in the tools disclosed herein may have an average grain size of less than 0.05 mm, preferably less than 0.04 mm, preferably less than 0.03 mm, preferably less than 0.028 mm, preferably less than 0.025 mm, preferably less than 0.02 mm, preferably less than 0.018 mm, preferably less than 0.015 mm, and preferably less than 0.010 mm.
[0186] The graphite material used in the tools disclosed herein may have an average grain size of greater than 0.001 mm, preferably greater than 0.003 mm, preferably greater than 0.006 mm, preferably greater than 0.008 mm, preferably greater than 0.010 mm, preferably greater than 0.012 mm, preferably greater than 0.014 mm, preferably greater than 0.020 mm, preferably greater than 0.025 mm, preferably greater than 0.030 mm.
[0187] The graphite material used in the tools disclosed herein has a hardness of 1.45 g / cm 3 More than 1.50 g / cm 3 More than 1.55 g / cm 3 More than 1.60 g / cm 3 More than 1.65 g / cm 3 More than 1.70 g / cm, preferably 1.70 g / cm 3 More than 1.75 g / cm 3 The density may be equal to or greater than 100 nm.
[0188] The graphite material used in the tools disclosed herein has a hardness of <2.0 g / cm 3 , preferably 1.90 g / cm 3 , preferably <1.85g / cm 3 , and preferably <1.80 g / cm 3 The density of the sintered body may be 0.01 to 0.01.
[0189] In an embodiment, the graphite material has a molecular weight of 3.3×10 -6 / ℃ or more, 3.5×10 -6 / ℃ or more, 3.7×10 -6 / ℃ or more, 4.0×10 -6 / ℃ or more, 4.2×10 -6 / ℃ or more, 4.4×10 -6 / ℃ or more, 4.6×10 -6 / ℃ or more, and 4.8×10 -6 400 to about 2,000°C (or at least up to about 1200°C as shown in the figure).
[0190] In an embodiment, the graphite material has a molecular weight of 7.2×10 -6 / ℃ or less, preferably 7.0×10 -6 / ℃ or less, preferably 6.0×10 -6 / ℃ or less, preferably 5.0×10 -6 / ℃ or less, preferably 4.8×10 -6 / °C or less, and preferably 4.6 x 10 -6 3. The material may have a coefficient of thermal expansion (CTE) over a temperature range of about 400 to about 2,000° C. (or at least up to about 1200° C., as shown in the figure) up to about 1 / ° C.
[0191] Table 1 lists the properties of exemplary graphite materials disclosed herein.
[0192] [Table 1]
[0193] The die system 2 includes a die 6 and, optionally but preferably, at least one conductive foil 7 disposed on the inner wall of the die, as shown in the embodiment of Figures 4A-4C. The number of conductive foils on the inner wall of the die is not limited, and 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 conductive foils may be provided as circumferential liners between the die 6 and the upper punch 4 and the lower punch 4', such that the inner wall 8 of the die system 2 (including at least one conductive foil, if at least one conductive foil is present) and the outer wall 11 of each of the upper and lower punches define the gap 3. The at least one conductive foil 7 may include graphite, niobium, nickel, molybdenum, platinum, and other ductile conductive materials, and combinations thereof, that are stable within the temperature range according to the methods disclosed herein.
[0194] In certain embodiments, the conductive foil may comprise a flexible and compressible graphite foil as disclosed herein having one or more of the following properties: ● a carbon content of greater than 99% by weight, preferably greater than 99.2% by weight, more preferably greater than 99.4% by weight, more preferably greater than 99.6% by weight, more preferably greater than 99.8% by weight, more preferably greater than 99.9% by weight, more preferably greater than 99.9% by weight, more preferably greater than 99.999% by weight; ● impurities less than 500 ppm, preferably less than 400 ppm, more preferably less than 300 ppm, more preferably less than 200 ppm, more preferably less than 100 ppm, more preferably less than 50 ppm, more preferably less than 10 ppm, more preferably less than 5 ppm, more preferably less than 3 ppm; a tensile strength of the graphite film in the range of 4.0 to 6.0 MPa, preferably 4.2 to 5.8 MPa, and more preferably 4.4 to 5.6 MPa; and / or The bulk density of the graphite foil preferably in the range of 1.0-1.2 g / cc, preferably 1.02-1.18 g / cc, more preferably 1.04-1.16 g / cc, more preferably 1.06-1.16 g / cc.
[0195] In embodiments, the at least one foil typically comprises graphite. In certain embodiments, the at least one foil as part of the die system may include circumferential liners between a surface of the die and each of the upper and lower punches.
[0196] The graphite foil can improve the temperature distribution across the powder during sintering. Table 2 lists the properties of exemplary graphite foils according to embodiments disclosed herein, such as Neograf Grafoil®, Sigraflex® graphite foil, and Toyo Tanso Perma-Foil®.
[0197] [Table 2]
[0198] 4A, 4B and 4C, an SPS tool set according to an embodiment of a graphite foil configuration is shown. Yttrium oxide powder 5 is disposed between at least one of the upper and lower punches 4 and 4', and a gap 3 is shown between the outer wall 11 of each of the upper and lower punches and the inner wall 8 of the die system 2. FIGS. 4A, 4B and 4C each show 1-3 layers 7 of conductive foil and a die 6 as part of the die system 2. Thus, the gap extends from the inner wall 8 of the die system 2 to the outer wall 11 of each of the upper and lower punches. The gap distance is arranged to maintain ohmic contact between the punch and die to improve temperature distribution throughout the yttria ceramic powder during heating and sintering while allowing the powder to degas before and / or during heating and sintering.
[0199] The thickness of the graphite foil 7 may be, for example, 0.025 to 0.260 mm, preferably 0.025 to 0.200 mm, preferably 0.025 to 0.175 mm, preferably 0.025 to 0.150 mm, preferably 0.025 to 0.125 mm, preferably 0.035 to 0.200 mm, preferably 0.045 to 0.200 mm, preferably 0.055 to 0.200 mm.
[0200] The distance of the gap 3 is measured from the inward facing surfaces of the foil 7 closest to the upper punch 4 and the lower punch 4' to the outer wall 11 of each of the upper and lower punches. Preferred ranges for the distance of the gap 3 are preferably 10-70 μm, preferably 10-60 μm, preferably 10-50 μm, preferably 20-70 μm, preferably 30-70 μm, preferably 40-70 μm, preferably 25-45 μm, preferably 20-60 μm, and preferably 30-60 μm.
[0201] Furthermore, the width of the gap 3 between the inner wall 8 of the die system 2 and the outer wall 11 of each of the upper and lower punches 4 and 4' can be determined by a person skilled in the art so that powder degassing during the preheating, heating and sintering process is sufficiently promoted on the one hand, and sufficient electrical contact for Joule or resistive heating and thereby sintering is achieved on the other hand. If the gap distance 3 is less than 10 μm, the force required to move at least one of the upper and lower punches in the internal volume of the die system and thereby assemble the tool set may cause damage to the tool set. Furthermore, a gap 3 less than 10 um may not allow gases, organics, moisture, etc. adsorbed in the yttria powder 5 to escape, which may extend the processing time during production and result in residual porosity in the sintered yttria ceramic body, thereby reducing the density. If the width of the gap 3 is greater than 70 μm when sintering insulating powders of yttrium oxide, local overheating may occur and thermal gradients may occur in the tool set during sintering. As a result, in order to form a large yttria sintered body, a gap of 10 to 70 μm is preferred. Therefore, in some embodiments, the distance of the gap 3 between the inner wall 8 of the die system 2 and the outer walls 11 of the upper and lower punches when sintering the yttrium oxide powder is preferably 10 to 70 μm, preferably 10 to 60 μm, preferably 10 to 50 μm, preferably 10 to 40 μm, preferably 20 to 70 μm, preferably 30 to 70 μm, preferably 40 to 70 μm, preferably 50 to 70 μm, preferably 30 to 60 μm.
[0202] These thermal gradients can result in low overall or bulk density and high density variation, as well as fragile and easily broken sintered yttrium oxide ceramic bodies. As a result, the gap 3 distance between the inner wall 8 of the die system 2 and the outer wall 11 of each of the upper and lower punches when sintering the yttrium oxide ceramic powder disclosed herein is 10 to 70 μm, preferably 10 to 60 μm, preferably 10 to 40 μm, preferably 20 to 70 μm, preferably 40 to 70 μm, preferably 50 to 70 μm, preferably 30 to 70 um, preferably 40 to 60 μm. Without intending to be bound by a particular theory, it is believed that the gap distance between the inner wall 8 of the die system 2 and the outer wall 11 of each of the upper and lower punches during sintering serves to facilitate powder outgassing of organics, moisture, adsorbed molecules, etc. during the sintering process. This results in large sized yttria sintered ceramic bodies having high density and low volume porosity, low density variation, and improved mechanical properties, and therefore can be easily handled without breakage. Sintered ceramic bodies made as disclosed herein can have dimensions of 100 mm to 610 mm, in some embodiments 100 mm to 625 mm, with respect to the maximum dimension of the sintered ceramic body.
[0203] In practice, the upper and lower punches 4 and 4' are not necessarily perfectly aligned with respect to the central axis. Figures 5A and 5B are plan views of the tool set 1, showing the alignment of the upper and lower punches 4 and 4', the gap 3, the number of conductive foils 7, and the die system 2 about the central axis 9. In the embodiment shown in Figure 5A, the gap may be axisymmetric with respect to the central axis 9. In other embodiments, such as depicted in Figure 5B, the gap may be asymmetric about the central axis 9. The gap 3 may extend from 10um to 70um, and in some embodiments from 10um to 100um, when sintering yttrium oxide powder to form the yttria sintered ceramic body disclosed herein, in both the axisymmetric and asymmetric embodiments shown.
[0204] Gap asymmetry performance can be measured by performing an absolute radial CTE deviation analysis over a temperature range. (CTE describes how an object changes size with a change in temperature. Specifically, it measures the rate of size change per degree of temperature change at constant pressure). For example, FIG. 6 shows the radial deviation from the average CTE of two isotropic graphite materials (A and B) used as punches and dies in the apparatus disclosed herein at 1200° C. FIG. 6 shows that for a material to be successful in maintaining a desired gap over a wide temperature range, the radial deviation must be >0.3×10 in the xy plane, e.g., from room temperature to 2000° C. -6 This shows that the CTE can vary from the average by only 1 / °C.
[0205] Thus, as disclosed herein, 1×10 +10 In order to maintain the desired gap 3 over the temperature range required to sinter insulating yttria powder having a resistivity of 0.3×10 or greater, the radial deviation from the average CTE may preferably be minimized, and thus the radial deviation is preferably less than 0.3×10 or greater over the temperature range of interest. -6 / ℃ or less, preferably 0.25×10 -6 / ℃ or less, preferably 0.2×10 -6 / ℃ or less, preferably 0.18×10 -6 / °C or less. In certain embodiments, -6 / ℃ or less, preferably 0.14×10 -6 / ℃ or less, preferably 0.12×10 -6 / ℃ or less, preferably 0.1×10 -6 / ℃ or less, preferably 0.08×10 -6 / ℃ or less, preferably 0.06×10 -6It may be preferred that a radial deviation from the average CTE of no more than 1 / °C be maintained to provide the desired gap 3 over a temperature range from room temperature to the sintering temperature of the ceramic powder, including up to the operating temperature of the apparatus of about 2,000°C. The disclosed ranges of radial deviation from the average CTE of the at least one graphite material in the xy plane should be maintained over rotational positions about the central axis 9 of 0-360 degrees, preferably 0-270 degrees, preferably 0-180 degrees, preferably 0-90 degrees, preferably 0-45 degrees, preferably less than 10 degrees, preferably less than 5 degrees, preferably about 3 degrees, and preferably about 1 degree for rotational positions of the die and the upper punch and / or lower punch, respectively.
[0206] Material B exhibited unacceptable CTE expansion in the xy plane, while material A exhibited acceptable CTE expansion across the entire temperature range. Figure 7a) shows the standard deviation (ppm / °C) of the CTE of the graphite materials, and b) shows the absolute variation (delta) of CTE across the xy plane (ppm / °C from lowest to highest) of both materials in Figure 6 across the temperature range. Figure 8 shows the variation of the thermal expansion coefficient of graphite materials A and B from 400°C to 1400°C. The required range of radial deviation from the average CTE can be applied across many different graphite materials having ranges of CTE expansion as disclosed herein, without limitation. Thus, graphite materials meeting the disclosed ranges of radial deviations can be found across a range of, for example, 4x10 -6 / ℃~7×10 -6 / °C range and may be useful in manufacturing punches 4, 4' and / or die 6. In an embodiment, the CTE of upper punch 4 and lower punch 4' is preferably equal to or less than the CTE of die 6. The table below shows the maximum radial excursion (maximum variation in CTE) in the xy plane, the average CTE, and the standard deviation of CTE for an exemplary material A. The average of the maximum variation in CTE over all temperatures was calculated to be 0.083 ppm / °C.
[0207] [Table 3]
[0208] The advantages of the particular toolset design used in accordance with one embodiment may result in the overall technical effect of providing large yttria ceramic bodies, in accordance with the present disclosure, that are of very high purity, have high uniform density and low volumetric porosity, and thereby have reduced tendency to break during sintering processes, particularly SPS processes, and therefore all of the features disclosed with respect to the toolset also apply to the production of sintered ceramic bodies with dimensions greater than 100 mm.
[0209] By using the toolset disclosed herein, it is possible to achieve a more uniform temperature distribution in the yttrium oxide powder 5 to be sintered and to produce yttria sintered ceramic bodies, especially those with large dimensions, e.g., with a maximum dimension exceeding 100 mm and / or 200 mm, with a very high (>98% of the theoretical density of yttrium oxide) uniform density (<4% variation across the maximum dimension), and thus with a reduced tendency to break. The term "homogeneous" means that the material or system has substantially the same properties at all points, being consistent and uniform. Thus, "uniform temperature distribution" means that the temperature distribution is spatially uniform and does not have significant gradients, i.e., there is a substantially uniform temperature regardless of the position in the horizontal xy plane along the ceramic powder 5.
[0210] A toolset as disclosed may further include spacer elements, shims, liners, and other toolset components, typically fabricated from at least one of the graphite materials having the properties disclosed herein.
[0211] Method for producing sintered yttrium oxide bodies The preparation of sintered yttrium oxide bodies may be accomplished through the use of pressure assisted sintering and related techniques in combination with direct current sintering, which uses direct current to heat an electrically conductive die arrangement or tool set and thereby heat the material to be sintered. This heating method allows for the application of very high heating and cooling rates, which can facilitate the preparation of very fine grain sintered yttrium oxide bodies, enhancing densification mechanisms over grain growth enhanced diffusion mechanisms, and transferring the inherent properties of the original powders to their nearly or fully dense products.
[0212] The above-mentioned properties of the corrosion-resistant sintered yttrium oxide body and components formed from the sintered yttrium oxide body are achieved by, among other things, tailoring the purity of the yttrium oxide powder, the surface area of the yttrium oxide powder, the heating and cooling rates of the yttrium oxide powder and the sintered body, the pressure applied to the yttrium oxide powder, the temperature of the yttrium oxide powder, the time of sintering the powder, the temperature of the sintered yttrium oxide body or component during the optional annealing step, and the time of the annealing step.
[0213] A process for producing a sintered yttrium oxide body is disclosed, the process comprising: a. disposing yttrium oxide powder within an interior volume defined by a spark plasma sintering tool, the spark plasma sintering tool comprising: a die including a sidewall including an inner wall having a diameter defining the interior volume, and an outer wall; and an upper punch and a lower punch operatively coupled to the die, each of the upper punch and the lower punch having an outer diameter smaller than the diameter of the inner wall of the die, thereby creating a gap between each of the upper punch and the lower punch and the inner wall of the die when at least one of the upper punch and the lower punch is moved within the interior volume of the die, the gap being between 10 μm and 70 μm in width, creating a vacuum condition within the interior volume; b. applying pressure to the yttrium oxide powder at a pressure of 10 MPa to 60 MPa by moving at least one of the upper punch and the lower punch within the internal volume of the die while heating the yttrium oxide powder to a sintering temperature of 1200 to 1600°C, thereby forming a sintered yttrium oxide body; c. Reducing the temperature of the sintered yttrium oxide body, wherein the yttrium oxide powder of step a) is reduced by 10 ml. 2 The sintered yttrium oxide body has a surface area of 4.93 g / cm3 or less and a total impurity level of 40 ppm or less. 3 or greater, and at least one surface contains at least one pore, each pore having a diameter of 5 μm or less.
[0214] The following additional steps: d. optionally annealing the sintered yttrium oxide body by increasing the temperature of the sintered yttrium oxide body to an annealing temperature; e. reducing the temperature of the annealed sintered yttrium oxide body; f. Optionally, machining the sintered yttrium oxide body to produce a sintered yttrium oxide body component, the component being selected from the group consisting of a dielectric or RF window, a focus ring, a nozzle or gas injector, a showerhead, a gas distribution plate, an etch chamber liner, a plasma source adaptor, a gas inlet adaptor, a diffuser, an electronic wafer chuck, a chuck, a puck, a mixing manifold, an ion suppressor element, a faceplate, an isolator, a spacer, and a guard ring; is as per need.
[0215] The sintering tool (the terms "tool" and "apparatus" are used interchangeably herein) may be a pressure-assisted sintering apparatus, such as a Spark Plasma Sintering (SPS) apparatus. SPS is also known as Field Assisted Sintering Technology (FAST) or Direct Current Sintering (DCS). DC and related techniques use direct current to heat a conductive die configuration and thereby the material to be sintered. This heating method allows for the application of very high heating and cooling rates, enhancing densification mechanisms over grain growth enhanced diffusion mechanisms, transferring the inherent properties of the original powders to their nearly or fully dense products.
[0216] The method is characterized in that the above-mentioned SPS toolset is placed in a vacuum chamber and includes at least a die system and an upper punch and a lower punch, which together define a volume, whereby a sintering process of the powder is performed by placing the powder in the volume defined by the sintering machine toolset. The die system may have an inner wall and the at least one punch system may have an outer wall, the inner wall of the die system and the outer wall of the punch system being separated by a gap.
[0217] Certain process steps will now be described in detail.
[0218] Process step (a) - Placing yttrium oxide powder within an interior volume defined by a tool set of a spark plasma sintering tool, the spark plasma sintering tool comprising a die including a sidewall including an inner wall having a diameter defining the interior volume, and an outer wall, and an upper punch and a lower punch operatively coupled to the die, each of the upper punch and the lower punch having an outer diameter smaller than the diameter of the inner wall of the die, thereby creating a gap between each of the upper punch and the lower punch and the inner wall of the die when at least one of the upper punch and the lower punch is moved within the interior volume of the die, the gap being between 10 μm and 70 μm wide, and creating a vacuum condition within the interior volume. The disclosed method utilizes commercially available yttrium oxide powder or one prepared from chemical synthesis techniques and does not require sintering aids, cold pressing, forming a green body or machining prior to sintering.
[0219] The yttrium oxide powder is loaded into a die of an SPS sintering apparatus, for example as disclosed above, where the spark plasma sintering tool includes a die including a sidewall including an inner wall and an outer wall, the inner wall having a diameter defining an interior volume, and an upper punch and a lower punch operatively connected to the die, each of the upper punch and the lower punch having an outer diameter smaller than the diameter of the inner wall of the die, thereby generating a gap between each of the upper punch and the lower punch and the inner wall of the die when at least one of the upper punch and the lower punch is moved within the interior volume of the die, the gap being between 10 μm and 70 μm in width. Vacuum conditions known to those skilled in the art are established within the powder disposed within the interior volume. Exemplary vacuum conditions include vacuum conditions of 10 μm to 70 μm in width. -2 ~10 -3 Pressures of up to 100 torr are used. The vacuum is applied primarily to remove the air to protect the graphite from burning and to remove most of the air from the powder.
[0220] The yttrium oxide starting material for carrying out the sintering process is a commercially available yttrium oxide powder with high purity. However, other yttrium oxide powders, such as those produced from chemical synthesis processes and related methods, can also be used. The purity of the yttrium oxide starting powder is preferably greater than 99.99%, more preferably greater than 99.998%, and most preferably greater than 99.999%. In some embodiments, the purity of the yttrium oxide starting powder is greater than 99.9999%. In other words, the total impurity level of the yttrium oxide powder can be less than 50 ppm, preferably less than 40 ppm, more preferably less than 30 ppm, more preferably less than 25 ppm, more preferably less than 20 ppm, more preferably less than 15 ppm, even more preferably less than 10 ppm, and even more preferably less than 6 ppm (including 0 ppm) in terms of total impurity level. A high purity starting powder is desirable for optimal etching performance in the finished sintered yttrium oxide body / component.
[0221] In contrast to other sintering techniques in the prior art, the yttrium oxide powder used in the process of the present disclosure does not contain sintering aids and polymer binders.
[0222] The average particle size of the yttrium oxide powder used as a starting material in the SPS process according to one embodiment of the present invention is usually 0.5-20 μm, preferably 1-15 μm, preferably 2-10 μm, and more preferably 5-8 μm.
[0223] Yttrium oxide powder is 10m 2 In some embodiments, the yttrium oxide powder has a surface area of 1.0 to 10.0 m 2 / g, preferably 1.5 to 8.0 m 2 / g, preferably 2 to 7, more preferably 2 to 5m 2 / g surface area.
[0224] Preferably, the yttrium oxide powder starting material is not ball milled prior to its use in the processes of the present invention, as ball milling is a potential source of contaminants / impurities.
[0225] In some embodiments, the yttrium oxide powder may be treated in a manner to remove undesirable moisture, organic matter or agglomerates. Such treatment may include tumbling, jet milling and / or sieving prior to its use in step a) of the process disclosed herein.
[0226] In embodiments, the yttrium oxide powder may be calcined prior to use in the processes of the present invention. Exemplary calcination temperatures include temperatures of about 600° C. to about 1000° C. in an oxygen-containing environment for a duration of 4 to 12 hours. Before and / or after calcination, the yttrium oxide powder may be sieved and / or tumbled without the use of grinding media according to known methods.
[0227] process step (b) - applying a pressure of 10 MPa to 60 MPa to the yttrium oxide powder by moving at least one of the upper punch and the lower punch within the internal volume of the die while heating the yttrium oxide powder to a sintering temperature of 1200 to 1600°C, thereby forming a sintered yttrium oxide body by sintering; and process step (c) - reducing the temperature of the sintered yttrium oxide body. After the yttrium oxide material is placed within the internal volume defined by the toolset of the spark plasma sintering tool and most of the air is removed from the die / powder, pressure is applied to the yttrium oxide material disposed between the graphite punches. The pressure is preferably increased to a pressure of 10 MPa to 60 MPa, preferably 10 MPa to 40 MPa, more preferably 15 MPa to 40 MPa, preferably 20 to 40 MPa, even more preferably 20 to 30 MPa.
[0228] Pressure is preferably applied axially to the material provided in the die. After applying pressure, the yttria powder forms a powder compact which may have a packing density of 20% to 60% by volume, 20% to 55% by volume, preferably 30% to 60% by volume, preferably 30% to 55% by volume, preferably 40% to 60% by volume, preferably 40% to 55% by volume. A higher packing density is desirable to improve thermal conductivity within the powder compact, thereby reducing temperature differences across the powder compact during heating and sintering.
[0229] In a preferred embodiment, the yttrium oxide powder is heated directly by the punch and die of the SPS apparatus. The die may be constructed of a conductive material such as graphite to facilitate resistive / joule heating. SPS apparatus and procedures are disclosed, for example, in U.S. Patent Application Publication No. 2010 / 0156008, which is incorporated herein by reference.
[0230] The application of heat to the yttrium oxide powder fed into the die facilitates a sintering temperature of about 1000-1700° C., preferably about 1200-1600° C., preferably about 1300-1550° C., preferably about 1350-1500° C., more preferably about 1400-1500° C. In one embodiment, sintering is accomplished for a time of 0-1440 minutes, in another embodiment, sintering is accomplished for a time of 0-720 minutes, in another embodiment, sintering is accomplished for a time of 0-360 minutes, in another embodiment, sintering is accomplished for a time of 0-240 minutes, in another embodiment, sintering is accomplished for a time of 0-120 minutes, in another embodiment, sintering is accomplished for a time of 0-60 minutes, in another embodiment, sintering is accomplished for a time of 0-30 minutes, in another embodiment, sintering is accomplished for a time of 0-20 minutes, in another embodiment, sintering is accomplished for a time of 0-10 minutes, and in another embodiment, sintering is accomplished for a time of 0-5 minutes.
[0231] The temperature of a sintering apparatus according to the present disclosure is typically measured in the graphite die of the apparatus, and therefore it is preferred that the temperature is measured as close as possible to the yttrium oxide being sintered so that the indicated temperature is actually realized in the yttrium oxide.
[0232] The order of application of pressure and temperature in one embodiment may be varied according to the present disclosure, meaning that it is possible to apply the indicated pressure first and then apply heat to achieve the desired temperature. Furthermore, in other embodiments, it is also possible to apply the indicated heat first to achieve the desired temperature and then apply the indicated pressure. In a third embodiment according to the present disclosure, the temperature and pressure may be applied simultaneously to the yttrium oxide to be sintered and increased until the indicated values are reached.
[0233] Induction or radiative heating methods can also be used to heat the sintering apparatus and indirectly heat the yttrium oxide powder in the toolset.
[0234] In contrast to other sintering techniques, no pre-sintering sample preparation, i.e. cold pressing or green body formation before sintering, is required and the powder is directly loaded into a mold, which may provide higher purity in the final sintered yttrium oxide body.
[0235] In further contrast to other sintering techniques, no sintering aids are required. Additionally, high purity starting powders are desirable. The absence of sintering aids and the use of high purity starting materials with purities of greater than 99.99% to 99.9999% permits the production of high purity sintered yttrium oxide bodies that provide improved etch resistance for use in semiconductor etch chambers.
[0236] In some embodiments, sintering under an isothermal residence time may be applied for a period of 0 minutes to 1440 minutes, in other embodiments, sintering under an isothermal residence time may be applied for 0 minutes to 720 minutes, in other embodiments, sintering under an isothermal residence time may be applied for 0 minutes to 360 minutes, in other embodiments, sintering under an isothermal residence time may be applied for 0 minutes to 240 minutes, in other embodiments, sintering under an isothermal residence time may be applied for 0 minutes to 120 minutes, in other embodiments, sintering under an isothermal residence time may be applied for 0 minutes to 60 minutes, in other embodiments, sintering under an isothermal residence time may be applied for 0 minutes to 30 minutes, in other embodiments, sintering under an isothermal residence time may be applied for 0 minutes to 20 minutes, in other embodiments, sintering under an isothermal residence time may be applied for 0 minutes to 10 minutes, and in other embodiments, sintering under an isothermal residence time may be applied for 0 minutes to 5 minutes.
[0237] In one embodiment of the present invention, the SPS process comprises a pre-sintering step with a specific heating gradient of 0.1°C / min-100°C / min, 0.25°C / min-50°C / min, preferably 0.5°C / min-50°C / min, preferably 0.75°C / min-50°C / min, preferably 1°C / min-50°C / min, more preferably 2-25°C / min, more preferably 3-20°C / min, preferably 4-15°C / min, preferably 5-10°C / min, until a specific pre-sintering time is reached.
[0238] In a further embodiment of the present invention, the SPS process step comprises a pre-sintering step with a specific pressure gradient of 0.10 MPa / min to 30 MPa / min, 0.2 to 25, preferably 0.25 to 20, 0.25 MPa / min to 15 MPa / min, preferably 0.5 to 10 MPa / min, preferably 1 to 10 MPa / min, until a specific pre-sintering time is reached.
[0239] In another embodiment of the present invention, the SPS process step includes a pre-sintering step using the specific heat lamps described above and the specific pressure lamps described above.
[0240] In process step (c), the sintered yttrium oxide may be passively cooled by removal of the heat source, allowing natural convection to occur, until a temperature is reached that may facilitate the optional annealing process. In a further embodiment, the sintered yttrium oxide body may be cooled under convection with an inert gas, for example argon or nitrogen at 1 bar. Other gas pressures, greater or less than 1 bar, may also be used. To initiate the cooling process, the power applied to the SPS apparatus may be removed. The pressure applied to the sintered sample is removed at the end of the SPS process before (natural) cooling occurs.
[0241] During sintering, a volume reduction typically occurs such that the sintered yttrium oxide body may contain approximately one-third the volume of the starting yttrium oxide powder when placed in the sintering apparatus toolset.
[0242] By using an SPS toolset having a range of gap dimensions as disclosed herein, the gap may be maintained throughout the method, particularly during the sintering step as disclosed, resistive overheating may be prevented, and this temperature difference may be minimized such that the density of the sintered ceramic body has minimal variation across the distance between the inner surface 8 of the die system and the central axis 9 defining the center. Uniform densification during sintering may result in density variations across the maximum dimension of the sintered ceramic body as disclosed herein that are preferably less than 4%, less than 3%, preferably less than 2%, preferably less than 1%, more preferably less than 0.5%, preferably 0.25-5%, preferably 0.25-4%, preferably 0.25-3%, preferably 0.25-2%, preferably 0.25-1%, preferably 0.25-0.5%, preferably 0.5-3.5%, and preferably 1-3% across the maximum dimension of the sintered ceramic body.
[0243] Further contributing to uniform densification during sintering is the high packing density of 30-60 volume percent of powder compacts including the yttrium oxide powders disclosed herein prior to sintering, which can be achieved using the disclosed yttria powders and methods.
[0244] The temperature of the sintering apparatus according to the present disclosure is typically measured in a die containing at least one graphite material of the sintering apparatus, and therefore it is preferred that the temperature is measured as close as possible to the ceramic powder to be sintered so that the indicated temperature is actually realized in the ceramic powder.
[0245] The order of application of pressure and temperature in one embodiment may be varied according to the present disclosure, meaning that it is possible to apply the indicated pressure first and then apply heat to achieve the desired temperature. Additionally, in other embodiments, it is also possible to apply the indicated heat first to achieve the desired temperature and then apply the indicated pressure. In a third embodiment according to the present disclosure, temperature and pressure may be applied simultaneously to the ceramic powder to be sintered and increased until the indicated values are reached.
[0246] Induction or radiative heating methods can also be used to heat the sintering apparatus and indirectly heat the yttria powder in the toolset.
[0247] In contrast to other sintering techniques, no preparation of the powder prior to sintering is required, i.e. by cold pressing or forming a green body using organic additives such as binders, dispersants, etc., prior to sintering, and the powder is loaded directly into the internal volume of a spark plasma sintering tool to form a powder compact without the use of organic additives. This reduced handling can provide higher purity in the final sintered yttria ceramic body.
[0248] According to an embodiment of process step b), the temperature and pressure are maintained for a period of 1 min to 360 min, preferably 1 min to 240 min, preferably 1 min to 120 min, preferably 1 min to 60 min, preferably 5 min to 360 min, preferably 10 min to 360 min, preferably 30 min to 360 min, preferably 45 min to 360 min, preferably 60 min to 360 min, and preferably 60 min to 90 min to carry out sintering.
[0249] According to the embodiment of process step (c) - reducing the temperature of the sintered yttrium oxide body, the sintered yttrium oxide body may be passively cooled by removing the heat source and natural convection occurs until a temperature is reached that can facilitate the optional annealing process. In a further embodiment, the sintered yttrium oxide body may be cooled under convection with an inert gas, for example argon or nitrogen at 1 bar. Other gas pressures, greater or less than 1 bar, may also be used. To start the cooling process, the power applied to the SPS apparatus may be removed. The pressure applied to the sintered sample is removed at the end of the SPS process before (natural) cooling occurs.
[0250] process step (d) - in an optional step, annealing the sintered yttrium oxide body by applying heat to elevate the temperature of the sintered yttrium oxide body to an annealing temperature; and process step (e) reducing the temperature of the annealed sintered yttrium oxide body to ambient temperature by removing the heat source applied to the sintered yttrium oxide body. In optional step (d), the resulting sintered yttrium oxide body of step (c) is subjected to an annealing process. The annealing can be carried out in a furnace outside the sintering apparatus, without removing the sintered yttrium oxide body from the apparatus, or within the sintering apparatus itself. For example, in one embodiment, the sintered yttrium oxide may be removed from the sintering apparatus after cooling according to process step (c), and the annealing process step may be carried out in a separate apparatus, such as a furnace. In other embodiments, for the purposes of annealing according to the present disclosure, the yttrium oxide sintered in step (b) may be subsequently annealed while still in the sintering apparatus, without the need to remove it from the sintering apparatus between the sintering step (b) and the optional annealing step (d).
[0251] Annealing results in an improvement of the chemical and physical properties of the sintered yttrium oxide body. The annealing step can be carried out by conventional methods used for annealing glasses, ceramics and metals, and the degree of refinement can be selected by the selection of the annealing temperature and the time for which the annealing is continued.
[0252] The optional annealing step (d) can be carried out at temperatures between 1200 and 1800° C., preferably between 1250 and 1700° C., more preferably between 1300 and 1650° C. At such temperatures, oxygen vacancies in the crystal structure can be modified back to stoichiometric proportions.
[0253] The step of annealing the sintered yttrium oxide can be completed in 5 minutes to 24 hours, preferably 20 minutes to 20 hours, and more preferably 60 minutes to 16 hours.
[0254] The optional annealing process step (d) is preferably carried out in an oxidizing atmosphere in air.
[0255] After optional process step (d) of annealing the sintered yttrium oxide, the temperature of the annealed sintered yttrium oxide is cooled to ambient temperature according to process steps (c) or (e). The sintered and annealed yttrium oxide body is dense and typically has an average grain size of 0.25 μm to 25 μm, preferably 0.5 to 20 μm, preferably 0.75 to 15 μm, preferably 1 to 10 μm, more preferably 1 to 5 μm.
[0256] The SPS process described above according to one embodiment is suitable for use in the preparation of large sintered yttrium oxide bodies. The disclosed process provides rapid powder consolidation and densification, retains small (less than 13 um) d50 grain size in the sintered body transferred from the starting powder material, and achieves high uniform density of greater than 98% of theoretical with minimal (<3%) density variation across the longest dimension. This combination of fine grain size, uniformity and high density provides high strength sintered yttrium oxide bodies of large dimensions suitable for machining, handling and use as components in semiconductor processing chambers. For example, in one embodiment, the sintered yttrium oxide bodies may be formed in disk shapes having dimensions ranging from 40 mm to 600 mm or 40 to 625 mm in size and ranging from 40 mm to 100 mm in thickness. In another embodiment, the sintered yttrium oxide bodies may be formed in disk shapes having diameters ranging from 100 mm to 600 mm or diameters ranging from 100 to 325 mm. In another embodiment, sintered yttrium oxide bodies having dimensions ranging from 100 mm to 406 mm may be formed. In other embodiments, the sintered yttrium oxide body has a size of 200 mm to 600 mm or 200 mm to 625 mm, preferably 300 to 600 mm or 300 to 625 mm, preferably 350 to 600 mm or 350 to 625 mm, preferably 400 to 600 mm or 400 to 625 mm, more preferably 450 to 600 mm or 450 to 625 mm, more preferably 500 to 600 mm or 500 to 625 mm, more preferably 550 to 600 mm or 550 to 625 mm, for at least one dimension, which may be the longest dimension of the sintered body, respectively.
[0257] Finally, according to process step (f), the sintered (or sintered and annealed) yttrium oxide body may then be machined as necessary into final sintered yttrium oxide components for use in plasma etch chambers, such as, for example, dielectric or RF windows, focus rings, nozzles or gas injectors, showerheads, gas distribution plates, etch chamber liners, plasma source adapters, gas inlet adapters, diffusers, electronic wafer chucks, chucks, pucks, mixing manifolds, ion suppressor elements, faceplates, isolators, spacers, and guard rings. Machining (or sintering and annealing) of the sintered yttrium oxide body to make sintered components may be performed according to methods known to those skilled in the art.
[0258] The methods disclosed herein provide improved control over maximum pore size, high density, density variation, high purity, improved mechanical strength, and therefore handleability of sintered yttrium oxide bodies / components, particularly for bodies of dimensions greater than, for example, 200-600 mm across their maximum dimension.
[0259] Thus, in one embodiment disclosed herein, total impurity levels of 40 ppm or less, 4.93 g / cm 3 A sintered yttrium oxide body having a density of at least 5 μm or greater is provided, the sintered yttrium oxide body having at least one surface containing at least one pore, each pore having a diameter of 5 μm or less, the sintered yttrium oxide body being prepared by the steps of: a. placing yttrium oxide powder within an interior volume defined by a tool set of a spark plasma sintering tool, the spark plasma sintering tool set including a die including a sidewall including an inner wall having a diameter defining the interior volume, and an outer wall, and an upper punch and a lower punch operatively coupled to the die, each of the upper punch and the lower punch having an outer diameter smaller than the diameter of the inner wall of the die, thereby creating a gap between each of the upper punch and the lower punch and the inner wall of the die when at least one of the upper punch and the lower punch is moved within the interior volume of the die, the gap being between 10 μm and 70 μm wide, and creating a vacuum condition within the interior volume; b. applying pressure to the yttrium oxide powder at a pressure of 10 MPa to 60 MPa by moving at least one of the upper punch and the lower punch within the internal volume of the die while heating the yttrium oxide powder to a sintering temperature of 1200 to 1600°C, thereby forming a sintered yttrium oxide body; c. Reducing the temperature of the sintered yttrium oxide body, wherein the yttrium oxide powder of step a) is reduced by 10 ml. 2 The sintered yttrium oxide body has a surface area of 4.93 g / cm3 or less and a total impurity level of 40 ppm or less. 3 at least one surface of the porous material comprises at least one pore, each pore having a diameter of 5 μm or less; It is produced by a process including:
[0260] The sintered yttrium oxide body thus obtained (including the annealed sintered yttrium oxide) can be used in a plasma etching apparatus. Most integrated circuit (IC) manufacturing processes typically include multiple manufacturing steps in which various layers can be successively formed, shaped, or otherwise modified. One way to form a layer can be to deposit a layer and then etch it. Typically, etching can include forming an etch mask over the underlying layer. The etch mask can have a specific pattern that can mask certain portions of the underlying layer while leaving other portions exposed. Etching can then remove the portions of the underlying layer exposed by the etch mask. In this way, the etch mask pattern can be transferred to the underlying layer.
[0261] Plasma etching is currently used to process semiconductor materials for their use in the manufacture of electronics. Small features can be etched into the surface of the semiconductor material to be more efficient or to improve certain properties when used in electronic devices. For example, plasma etching can be used to create deep trenches on the surface of silicon for use in microelectromechanical systems. The application suggests that plasma etching may also play a major role in the manufacture of microelectronics. Similarly, research is currently being conducted into how the process can be tuned to the nanometer scale.
[0262] Plasma etching is usually performed in a plasma etch chamber that is commonly used to etch one or more layers formed on a semiconductor substrate that is typically supported on a substrate support within the chamber.
[0263] During plasma etching, a plasma is formed above the surface of the substrate by supplying radio frequency (RF) electromagnetic radiation to a low pressure gas (or gas mixture). By adjusting the potential of the substrate, charged species in the plasma can be directed to impinge on the surface of the substrate, thereby removing material (e.g., atoms) therefrom.
[0264] Plasma etching can be made more effective by using gases that chemically react with the material being etched. So-called "reactive ion etching" combines the energetic bombardment effect of a plasma with the chemical etching effect of reactive gases.
[0265] Sintered yttrium oxide according to one embodiment of the present disclosure may be used to fabricate plasma chamber components. Such components may have advantages including long life in aggressive etching conditions, since they can be made dense and highly pure by sintering using the SPS process described above. Sintered yttrium oxide bodies have many advantages in the context of plasma processing, including resistance to particle generation, improved plasma etching resistance, and enhanced part life. In addition, cleaning of yttrium oxide parts may be easier, since it may be possible to use aggressive cleaning methods, such as highly corrosive or aggressive chemicals.
[0266] Examples of chamber components that can be formed from the sintered yttrium oxide bodies disclosed herein include electrostatic chucks (ESCs), rings (e.g., process kit rings or single rings), chamber wall liners, bases, gas distribution plates, showerheads, liners, liner kits, shields, plasma screens, flow equalizers, cooling bases, chamber viewports, chamber lids, and the like.
[0267] In one embodiment, a processing chamber according to an embodiment of the present disclosure includes a chamber body and a showerhead that enclose an internal volume. Alternatively, the showerhead may be replaced by a lid and a nozzle, and the lid and nozzle may also be prepared from the above-mentioned yttrium oxide, either as a complete material or as a coating. The chamber body may be manufactured from aluminum, stainless steel, or other suitable materials. The chamber body generally includes a sidewall, a focus ring or edge ring that surrounds the wafer, and a bottom. One or more of the showerhead (or lid and / or nozzle), the sidewall, and / or the bottom include sintered yttrium oxide according to an embodiment of the present disclosure.
[0268] The features and advantages are more fully illustrated by the illustrative examples described below.
[0269] Working Example The following examples are included to more clearly demonstrate the general nature of the present disclosure. These examples are illustrative of the disclosure, but not limiting.
[0270] All particle size measurements were performed using a Horiba model LA-960 Laser Scattering Particle Size Distribution Analyzer, capable of measuring particle sizes from 10 nm to 5 mm. All specific surface area (SSA) measurements for the starting powders, powder blends, and calcined powder blends were performed in the range of 0.01 to 2000 m with an accuracy of 10% or better for most samples. 2 The measurements were performed using a Horiba BET Surface Area Analyzer model SA-9601 capable of measuring over a specific surface area of 1×10 / g. Purity and impurities were measured using an ICP-MS from an Agilent 7900 ICP-MS model G8403. All density measurements were performed according to ASTM B962-17 based on the Archimedes method known to those skilled in the art. The yttrium oxide powders and ceramics formed therefrom according to the examples have a specific surface area of about 1×10 +10 It is known to be an essentially insulating, highly resistive material with a resistivity of greater than ohm-cm.
[0271] Comparative Example 1: Specific surface area is 4.5 to 6.5 m 2 Polycrystalline ceramic sintered bodies with a maximum dimension of 406 mm were produced from a crystalline powder of yttrium oxide having a molecular weight of 1.5-3.5 μm, a d50 grain size of 4-6 μm, and a d90 grain size of 6.5-8.5 μm. The powder had a total impurity of about 14 ppm based on the total mass of the yttrium oxide powder. The die of the spark plasma sintering tool was lined with at least one graphite foil having the properties disclosed herein, and each of the die and the upper and lower punches of the tool included at least one graphite material disclosed herein. The powder was disposed within an interior volume defined by the spark plasma sintering tool, and the tool had a gap of about 100 μm. The gap was configured between an inwardly facing surface of the at least one graphite foil and an outer wall of each of the upper and lower punches of the spark plasma sintering tool. 10 -2 ~10 -3 A vacuum condition of 1000 torr was created inside the internal volume. The powder was sintered at 1,400° C. and 20 MPa pressure for 30 minutes to form a disk-shaped sintered ceramic body having a maximum dimension or diameter of 406 mm. The overall density of the sample was measured as 4.78 g / cc, or 95.03% of the theoretical density of yttrium oxide (reported as 5.03 g / cc). The density variation was measured to be about 4.5% relative to the highest density measurement across the maximum dimension. Sintered ceramic bodies prepared using a spark plasma sintering tool with gaps as disclosed in accordance with this example resulted in low overall density, high density variation, and subsequent fracture of the sintered body.
[0272] Example 1 (Sample 353 High Density, Large Size Polycrystalline Sintered Ceramic Body): Sintered ceramic bodies with a maximum dimension of 406 mm were prepared from a crystalline powder of yttrium oxide having a specific surface area of 6-8 m2 / g, a d10 grain size of 1-3 μm, a d50 grain size of 4-6 μm, and a d90 grain size of 7.5-9.5 μm. The powder had a total impurity of about 25 ppm based on the total mass of the yttrium oxide powder. The die of the spark plasma sintering tool was lined with at least one graphite foil having the properties disclosed herein, and the die and each of the upper and lower punches included at least one graphite material disclosed herein. The yttria powder was disposed within an interior volume defined by the spark plasma sintering tool with a gap of about 50 to about 70 μm, the gap being configured between an inwardly facing surface of the at least one graphite foil and an outer wall of each of the upper and lower punches of the sintering tool. The pre-pressing of the yttrium oxide powder was performed at a temperature of about 1000° C. -2 ~10 -3 The process was a multi-step process in which a pre-pressing pressure of about 10 MPa was applied under a vacuum of 1000 torr to form a powder compact having a packing density of about 35-45% by volume. The powder compact was sintered at a temperature of 1,550°C and a pressure of 20 MPa for 60 minutes. The radial variance from the average coefficient of thermal expansion (CTE) of at least one graphite material including the die and / or upper and lower punches about the central axis of the sintering tool was about 0.2×10 -6 / °C. The average density over five measurements was determined to be 5.020 g / cc, or 99.80% of the theoretical density of yttrium oxide (the theoretical density of yttrium oxide is 5.03 g / cm3 per DRLide, CRC Handbook of Chemistry and Physics, 84th Edition, 2012 ("the CRC Handbook"). Thus, tools having the specified gap distances and radial variations as disclosed herein can be used to form high density sintered ceramics of large dimensions.
[0273] Example 2 (Sample 152 Polycrystalline Yttrium Oxide Sintered Ceramic Body): A 100 mm sintered yttrium oxide body was formed from yttrium oxide powder having a surface area of 6.5-8.0 m2 / g and a purity of 99.999% (corresponding to an average total impurity of 18 ppm based on the total mass of the yttrium oxide powder). The d10 grain size was 1.5-3.5 μm, the median grain size (d50) was 4-6 μm, and the d90 grain size was 7.5-9.5 μm. The die of the spark plasma sintering tool was lined with at least one graphite foil having the properties disclosed herein, and each of the die and the upper and lower punches of the tool included at least one graphite material disclosed herein. The yttria powder was placed within an internal volume defined by the sintering tool, and a vacuum condition of 10-2-10-3 torr was created within the internal volume. The tool has a gap of about 25 to about 50 μm, the gap being configured between an inwardly facing surface of the at least one graphite foil and an outer wall of each of the upper and lower punches of the sintering tool. The radial variance of the average coefficient of thermal expansion (CTE) of the at least one graphite material comprising the die and / or the upper and lower punches about the central axis of the sintering tool is about 0.2×10 -6 The thermal expansion coefficient was determined to be less than 1.0 / °C. Sintering was performed at 1,400°C for 30 minutes at 30 MPa. This was followed by annealing in air at 1,400°C for 8 hours. An average density of 5.02 g / cc was measured, which corresponds to 99.9% of the theoretical density of yttrium oxide.
[0274] The following yttrium oxide samples, H1 / 66-H4 / 152, according to one embodiment of the present invention were prepared and compared with yttrium oxide samples, CM1 / 107, CM2 / 108 and 118, which were not prepared according to the present disclosure.
[0275] H1 / 66: A 80 mm sintered yttrium oxide body was placed on a 2.89 m 2The bodies were fabricated from powders with a surface area of 0.1 μm / g, a d50 grain size of 5.4 um, less than 10 ppm TREO (total rare earth oxides) and 48 ppm total impurities, with a powder purity of 99.9952%. The bodies were formed at a sintering temperature of 1500°C for 60 minutes at 30 MPa. Annealing was performed in air with a temperature ramp of 5°C / min to 1450°C for 1 hour, then at 1400°C for 8 hours. The density of the sintered yttrium oxide body was 4.948 g / cm 3 The maximum pore size was 1.1 um. The d10, d50 and d90 particle sizes were measured at 0.5, 0.8 and 1.4 um, respectively.
[0276] H2 / 65: Sintering temperature 1550°C, 30 MPa for 10 min, surface area 6.84 m 2 A 40 mm yttrium oxide sample was formed from 1000 g of powder. Annealing was performed in a furnace at a temperature of 1300° C. for 4 hours in air. The starting yttrium oxide powder had a total purity of 99.999%, corresponding to 10 ppm. The median particle size was measured to be 5.82 μm. The sintered yttrium oxide body had a total impurity level of 11 ppm. The purity of the starting powder was maintained in the sintered yttrium oxide body, indicating very little to no contaminants introduced during processing. The d10, d50 and d90 particle sizes were measured to be 4.0, 13.0 and 27.1 um, respectively, with an average particle size measured to be 14 um.
[0277] H3 / 79: A 40 mm sintered yttrium oxide body was placed on a 3.33 m 2The yttrium oxide bodies were formed from powders having a surface area of 0.1 μm / g and a median (d50) particle size of 5.17 μm. The starting powder had a total impurity of 2-4 ppm. Sintering of the yttrium oxide bodies was carried out using a sintering temperature of 1500°C for 10 minutes at a pressure of 30 MPa. The temperature was increased at 50°C / min while simultaneously applying pressure at 5 MPa / min. Annealing was carried out by increasing the temperature to 1300°C at 5°C / min and holding in air for 4 hours. The sintered yttrium oxide bodies had a total impurity level of 9-10 ppm, indicating minimal introduction of contaminants as a result of the process. The maximum pore size was measured to be 0.6 um and the density was measured to be 5.03 g / cc. The d10, d50 and d90 particle sizes were measured to be 0.8, 1.4 and 2.4 um, respectively. An average particle size of 1.47 um was also measured.
[0278] H4 / 152: 6.95m 2 A 100 mm sintered yttrium oxide body was formed from powder with a surface area of 0.01 g / g, 99.999% purity TREO (<10 ppm) and average total impurities of 18 ppm. The median grain size (d50) was 4.65 μm. Sintering was performed at 1400°C for 30 minutes at 30 MPa. Subsequent annealing was performed in air at 1400°C for 8 hours. 5.024 g / cm 3 After the two-step CF4 / O2 etching process as disclosed herein, the average step height of 0.98 um, the average etch rate of 0.68 nm / min, and the average pore size of 340,000 um were measured. 3 An etch volume of 1000 μm was obtained. Arithmetic mean heights (Sa) of 10 nm and 14 nm, respectively, were measured before and after the two-step CF4 / O2 etching process disclosed herein. After the oxygen etching process disclosed herein, an average step height of 0.1 μm, an average etch rate of 0.07 nm / min, and an average step height of 30,000 μm were measured. 3 After the SF6 etching process as disclosed herein, an average step height of 0.28 um, an average etch rate of 0.19 nm / min, and an etch volume of 90,000 um were obtained. 3 The etching volume was obtained.
[0279] Single-step, CF4 etching procedure To evaluate the etching performance, polished ceramic samples with dimensions of 6 mm × 6 mm × 2 mm were mounted on a c-plane sapphire wafer using a silicone-based heat sink compound. Areas of each section were shielded from exposure to the etching process by bonding a 5 mm × 5 mm square piece of sapphire ceramic to the sample surface.
[0280] The dry etch process was performed using a Plasma-Therm Versaline DESC PDC Deep Silicon Etch, an industry standard equipment. The etch was completed in 4 hour etch segments for a total time of 24 hours. The process was performed at a pressure of 10 millitorr, a CF4 flow rate of 90 standard cubic centimeters per minute (sccm), an oxygen flow rate of 30 sccm, and an argon flow rate of 20 sccm. The bias was 600 volts and 2000 watts ICP power. This etch recipe has a silicon etch rate of 512 nm / min. The etch recipe etches fused silica (quartz glass) at a rate of 72 nm / min. The etch conditions used herein to evaluate sample performance were selected to subject the disclosed materials to extreme etch conditions in order to differentiate performance.
[0281] Upon completion of the etching procedure, the surface roughness was measured.
[0282] Single-step, CF4 etching volume procedure: In one embodiment, the sintered yttrium oxide body has a diameter of about 12000 μm. 3 Less than about 9000 μm, preferably 3 less than about 7000 μm, more preferably 3 The etching volume is characterized by an etching rate of less than 90 standard cubic centimeters per minute at a pressure of 10 millitorr for a sample with dimensions of 6 mm x 6 mm x 2 mm. sccmThis is achieved when the etching process is performed as a reference process, which is subjected to etching conditions of CF4 flow rate of 1000 nm, oxygen flow rate of 30 standard cubic centimeters per minute (sccm), and argon flow rate of 20 standard cubic centimeters per minute (sccm), bias of 600 volts, and ICP power of 2000 watts for 24 hours. Each etching process is described in more detail in the experimental section below. The etched volume is thereby related to the volume of the yttrium oxide body removed during the indicated etching process.
[0283] Single-step, CF4 etch rate procedure: In some embodiments, the yttrium oxide body is characterized by an etch rate of less than about 0.08 nm / min, preferably less than about 0.06 nm / min, and more preferably less than about 0.05 nm / min, which is determined by a sample measuring 6 mm by 6 mm by 2 mm at a pressure of 10 millitorr and an etch rate of 90 standard cubic centimeters per minute. sccm This is achieved when a single-step CF4 etch process is performed as a reference process, with a CF4 flow rate of 1000 nm, an oxygen flow rate of 30 standard cubic centimeters per minute (sccm), and an argon flow rate of 20 standard cubic centimeters per minute (sccm), exposed to etching conditions for a period of 24 hours at a bias of 600 volts and an ICP power of 2000 watts, whereby the etch rate is related to the thickness reduction of the yttrium oxide body removed during the indicated etch process.
[0284] Single-step CF4Sdr procedure (unetched, etched) In some embodiments, the sintered yttrium oxide body has a 100x10 sintered area in accordance with ISO standard 25178-2-2012, section 4.3.2. -5 Less than 75x10, preferably -5 Less than 50x10, most preferably -5 and in the etched area, have a developed interface area ratio of less than 600x10 in accordance with ISO standard 25178-2-2012, section 4.3.2. -5Less than 500x10 -5 Less than 400x10 -5 Less than 300x10 -5 Less than 200x10, most preferably -5 The developed interface area ratio is characterized as being less than 100 nm. This latter developed interface ratio is achieved when a sample of a yttrium oxide body having dimensions of 6 mm x 6 mm x 2 mm is subjected to etching conditions of CF4 flow rate of 90 standard cubic centimeters per minute (sccm), oxygen flow rate of 30 standard cubic centimeters per minute (sccm), and argon flow rate of 20 standard cubic centimeters per minute (sccm) at a pressure of 10 millitorr, a bias of 600 volts, and an ICP power of 2000 watts, for a CF4 etch time of 24 hours. Each etching process is described in further detail below.
[0285] Single-step CF4Sa (unetched, etched). In some embodiments, the sintered yttrium oxide body is further characterized by having an arithmetic mean height Sa of less than 30 nm, more preferably less than 28 nm, and most preferably less than 25 nm, according to ISO standard 25178-2-2012, section 4.1.7, and an arithmetic mean height Sa of less than 40 nm, more preferably less than 35 nm, and most preferably less than 30 nm, according to ISO standard 25178-2-2012, section 4.1.7. The latter arithmetic mean height Sa is achieved when a sample of the yttrium oxide body having dimensions of 6 mm x 6 mm x 2 mm is subjected to etching conditions of 90 standard cubic centimeters per minute (sccm) CF4 flow rate, 30 standard cubic centimeters per minute (sccm) oxygen flow rate, and 20 standard cubic centimeters per minute (sccm) argon flow rate, 600 volts bias, and 2000 watts ICP power, at a pressure of 10 millitorr, for 24 hours. Each etching process is described in more detail below.
[0286] Surface roughness measurement Surface roughness measurements were performed using a Keyence 3D laser scanning confocal digital microscope model VK-X250X under ambient conditions in a Class 1 cleanroom. The microscope is placed on a TMC tabletop CSP passive benchtop isolator with a natural frequency of 2.8 Hz.
[0287] This non-contact system uses a laser beam light and an optical sensor to analyze a surface through reflected light intensity. The microscope acquires 1,024 data points in the x-direction and 786 data points in the y-direction for a total of 786,432 data points. Once a given scan is completed, the objective lens moves a set pitch in the z-direction and the intensity is compared between scans to determine focus. ISO 25178 Surface Texture (Areal Roughness Measurement) is the set of international standards for the analysis of surface roughness that this microscope complies with.
[0288] The surface of the sample was laser scanned using a confocal microscope at 10x magnification to capture detailed images of the sample. Line roughness was obtained on the profiles of the seven segmented blocks. Lambda chi (λ), which represents the measurement sampling length, was adjusted such that the line readings were limited to measurements from the five central blocks of the seven blocks, according to ISO standard 4288: Geometrical Product Specifications (GPS)--Surface texture:Profile method--Rules and procedures for the assessment of surface texture.
[0289] An area was selected within the etched and masked region of the sample for measurement. The area was chosen to be most representative of a typical sample surface and was used to calculate Sa and Sdr.
[0290] Surface roughness Sa and Sdr are parameters well known in the underlying technical field and are described, for example, in ISO standard 25178-2-2012, sections 4.1.7 (surface roughness Sa) and 4.3.2 (surface roughness Sdr).
[0291] Step measurement The step height as a result of the etching process is directly measured by using a Keyence 3D laser scanning confocal digital microscope model VK-X250X at 20x magnification. Selected areas in the etched and non-etched areas of the sample were used to create separate reference planes. The average height difference between these reference planes over three measurements can be considered as the step height.
[0292] Etch rate calculation The average etch rate in nanometers / hour can be calculated from the average step height by dividing the step height by the total etch time to arrive at the etch rate in nanometers / minute.
[0293] Volume measurement The etched volume was calculated from measurements at 50x on a Keyence 3D laser scanning confocal digital microscope model VK-X250X. A 7x7 image template is created from which a 7x1 region is selected for measurement. A reference plane is first established on a representative area of the masked and therefore unetched specimen. To establish the reference plane, an area within the masked region is selected. A tilt correction, enabled by the software, is completed over the region to account for variations in specimen thickness and mounting. A total area of 600um x 200um is then selected in the etched region of the image at the maximum distance from the masked surface. The height of the etched surface compared to a reference plane made on the masked surface is measured and the volume of material removed by etching relative to the reference plane is calculated over the selected region.
[0294] Difference between Ra and Sa measurements: Sa is the arithmetic mean height of the surface and is described in ISO 25178: Geometric Product Specifications (GPS) - Surface texture:area, an International Organization for Standardization collection on the analysis of 3D area surface textures. It is based on non-contact laser microscopy.
[0295] Ra is the arithmetic mean roughness of a 2D profile according to ISO 4287:1997 Geometrical Product Specifications (GPS)-Surface texture:Profile method. It is based on a mechanical stylus contacting the surface to create a linear profile.
[0296] Sa represents the height difference across the 3D measurement surface, and Ra represents the height difference across the 2D linear profile scan.
[0297] Ra is limited by the geometry of the stylus tip and can therefore result in loss of fine feature detail and distortion of peaks and valleys, which is problematic when measuring fine sub-micron features and is a limitation in using Ra values to compare with Sa values.
[0298] Additional samples were made according to the process of the present invention and are summarized in the table below, where applicable they are compared to commercial quartz (TSC 03) and comparative yttrium oxide samples (107, 108, and 118).
[0299] As an example, sample 188-1 was prepared as follows: 2Yttrium oxide powder having a surface area of 1 / g and 13 ppm total impurities corresponding to a powder purity of 99.9987% was used to form a 100 mm sintered yttrium oxide body. The pre-pressure was performed in a multi-step process whereby a pre-pressure of 20 MPa was applied under vacuum. Then, 5 MPa was applied while heating from room temperature to 600°C at a rate of 10°C / min. The pressure was increased to 30 MPa at a rate of 10°C / min between 600°C and the sintering temperature. Sintering was performed at a temperature of 1400°C and a pressure of 30 MPa for 30 minutes to complete the sintering. After sintering, the power to the sintering machine was cut off and allowed to cool naturally. Annealing was performed at a temperature of 1400°C for 8 hours in an oxygen-containing environment. The density was 5.002 g / cm. 3 It was.
[0300] In another example, sample 116 was prepared as follows: A 40 mm yttrium oxide sample was sintered at 1550° C. for 10 minutes at 30 MPa with a 6.84 mm 2 The sintered yttrium oxide body had a total impurity level of 11 ppm. The purity of the starting powder was maintained in the sintered yttrium oxide body, indicating very little or no contaminants introduced during processing. The d10, d50 and d90 particle sizes were measured to be 0.7, 6.7 and 25.4 um, respectively.
[0301] In another example, sample 224 was prepared as follows. 2Yttrium oxide powder having a surface area of 100 μm / g and an average of 8 ppm total impurities corresponding to a powder purity of 99.9992% was used to form a 100 mm sintered yttrium oxide body. Pressure was pre-applied at 20 MPa for approximately 5 minutes and a vacuum of 50 mTorr was established. The pressure was then reduced to 5 MPa and heated to 600° C. at a rate of 10° C. / min. Heat and pressure were applied simultaneously to reach a pressure of 20 MPa and the temperature was increased to 1400° C. at a rate of 10° C. / min. Sintering was carried out at a temperature of 1400° C. and a pressure of 20 MPa for 30 minutes to complete the sintering. After sintering, the power to the sintering machine was turned off and allowed to cool naturally. The sintered yttrium oxide body had d10, d50 and d90 particle sizes of 0.4, 0.7 and 1.2 um, respectively.
[0302] In another example, sample 189-1 was prepared as follows: 2 A 100 mm sintered yttrium oxide body was formed using yttrium oxide powder having a surface area of 1 / g and a total impurity of 24.8 ppm, corresponding to a powder purity of 99.9975%. Pressure preapplication was performed in a multi-step process whereby a pressure of 20 MPa was preapplication under vacuum. Then, 5 MPa was applied while heating from room temperature to 600°C at a rate of 10°C / min. The pressure was increased to 30 MPa at a rate of 10°C / min between 600°C and the sintering temperature. Sintering was performed at a temperature of 1400°C and a pressure of 30 MPa for 30 minutes to complete the sintering. After sintering, the power to the sintering machine was cut off and allowed to cool naturally. Annealing was performed at a temperature of 1400°C for 8 hours in an oxygen-containing environment. The impurity of the sintered yttrium oxide body was 36 ppm and the purity was 99.996%. The density of the annealed and sintered yttrium oxide body was 5.006 g / cm 3 After the two-step CF4 / O2 etching process as disclosed herein, the average step height was 0.82 um, the average etch rate was 0.57 nm / min, and the maximum pore size was 270,000 um. 3 The etching volume was obtained.
[0303] In another example, sample 045 was prepared as follows: 9-10m2 A 100 mm sintered yttrium oxide body was formed using yttrium oxide powder having a surface area of 0.1 μm / g and 26 ppm total impurities corresponding to a powder purity of 99.9974%. As disclosed herein, pre-pressure was applied in a multi-step process whereby a pre-pressure of 20 MPa was applied under vacuum. Then, 5 MPa was applied while heating from room temperature to 600° C. at a rate of 10° C. / min. The pressure was increased to 30 MPa at a rate of 10° C. / min between 600° C. and the sintering temperature. Sintering was carried out at a temperature of 1400° C. and a pressure of 30 MPa for 30 minutes to complete the sintering. After sintering, the power to the sintering machine was shut off and allowed to cool naturally. The average density was measured by Archimedes method to be 5.021 g / cm. 3 The annealing was carried out at a temperature of 1400 °C for 8 hours in an oxygen-containing environment. The average density after annealing was measured by Archimedes method and found to be 5.010 g / cm 3 It was.
[0304] In another example, sample 200-1 was prepared as follows: 2 A 150 mm sintered yttrium oxide body was formed using yttrium oxide powder having a surface area of 1 / g and total impurities of 9.5 ppm, corresponding to a powder purity of 99.9991%. Pressure was pre-applied at 20 MPa for approximately 5 minutes. It was then depressurized to 5 MPa and heated to 600°C at a rate of 25°C / min. Simultaneous application of heat and pressure was performed at a heating rate of 25°C / min and a pressure rate of 5 MPa / min up to 1000°C and 20 MPa. Heating was performed at a rate of 10°C / min between 1000°C and the sintering temperature. Sintering was performed at a temperature of 1400°C and a pressure of 20 MPa for 30 minutes to complete the sintering. After sintering, the power to the sintering machine was shut off and allowed to cool naturally. Annealing was performed at a temperature of 1400°C for 8 hours in an oxygen-containing environment. The density of the annealed and sintered yttrium oxide body was 4.945 g / cm 3 After the two-step CF4 / O2 etching process as disclosed herein, the average step height was 0.2 um, the average etch rate was 0.14 nm / min, and the maximum pore size was 60,000 um.3 After the oxygen etching process disclosed herein, an average step height of 0.1 um, an average etch rate of 0.07 nm / min, and an etch volume of 30,000 um were obtained. 3 After the SF6 etching process as disclosed herein, an average step height of 0.27 um, an average etch rate of 0.19 nm / min, and an etch volume of 80,000 um3 were obtained.
[0305] In another example, sample 212-1 was prepared as follows: 2 A 100 mm sintered yttrium oxide body was formed using yttrium oxide powder having a surface area of 100 μg / g and a total impurity of 8.1 ppm, corresponding to a powder purity of 99.9992%. Pressure was pre-applied at 20 MPa for approximately 5 minutes and a vacuum of 50 mTorr was established. It was then depressurized to 5 MPa and heated to 600°C at a rate of 50°C / min. Simultaneous application of heat and pressure was performed at a pressure rate of 10 MPa / min and temperature application was performed at a rate of 25°C / min to 30 MPa and 1450°C. Sintering was performed at a temperature of 1450°C and a pressure of 30 MPa for 30 minutes to complete the sintering. After sintering, the power to the sintering machine was cut off and allowed to cool naturally. Annealing was performed at a temperature of 1400°C for 8 hours in an oxygen-containing environment. The density of the annealed and sintered yttrium oxide body was 5.022 g / cm 3 The sintered yttrium oxide body had a total average impurities of 6 ppm, corresponding to a purity of 99.9994%. After a two-step CF4 / O2 etching process as disclosed herein, the body had an average step height of 1.1 um, an average etch rate of 0.77 nm / min, and a maximum pore size of 358,000 um. 3 The etching volume was obtained.
[0306] In another example, sample 314 was prepared as follows: 2Yttrium oxide powder having a surface area of 1 / g and 24.8 ppm total impurities corresponding to a powder purity of 99.9975% was used to form a sintered yttrium oxide body having a longest dimension of 406 mm. Pressure was pre-applied at 5 MPa and the temperature was ramped from room temperature to 800°C at 10°C / min. Simultaneous application of heat and pressure was performed with a heating rate of 10°C / min and a pressure ramp of 20 MPa from 800°C to 1000°C. Pressure was maintained at 20 MPa from 1000°C to the sintering temperature at a heating rate of 10°C / min. Sintering was performed at a temperature of 1450°C and a pressure of 20 MPa for a sintering duration of 60 minutes. Heating and pressing was terminated after the sintering period and natural cooling occurred. The sintered yttrium oxide body was annealed in an oxygen-containing environment at 1400°C for 8 hours using heating and cooling rates of 0.8°C / min. The average density of the annealed and sintered yttrium oxide body was 4.935 g / cm 3 and the density range across the longest dimension is 4.898-4.970 g / cm 3 It was.
[0307] In another example, sample 457 was prepared as follows: 2 Yttrium oxide powder having a surface area of 50 / g and 17 ppm total impurities corresponding to a powder purity of 99.9983% was used to form a sintered yttrium oxide body having a longest dimension of 406 mm. The powder was fired at 600° C. for 8 hours at 5-6 mm. 2The sintering was carried out at a surface area of 1 / g. Pressure was pre-applied at 5 MPa and the temperature was ramped from room temperature to 600°C at 10°C / min. Simultaneous application of heat and pressure was carried out with a heating rate of 5°C / min and a pressure ramp of 30 MPa from 600°C to 1000°C. Pressure was maintained at 30 MPa from 1000°C to the sintering temperature with a heating rate of 5°C / min. Sintering was carried out at a temperature of 1475°C and a pressure of 30 MPa for a sintering duration of 60 minutes. After the sintering time, the pressure was removed. Cooling was carried out using forced convection at 50% blower power for about 4 hours. Cooling using various blower power levels from about 25% to 100% allows forced convection cooling rates of 2.5°C / min to 5°C / min. Sintering was carried out at a temperature of 1475°C and a pressure of 30 MPa for a duration of 60 minutes. The sintered yttrium oxide bodies were annealed at 1400°C for 4 hours in an oxygen-containing environment using a heating rate of 0.8°C / min and a cooling rate of 2°C / min. The average density of the annealed and sintered yttrium oxide bodies was 4.985 g / cm 3 and the density range across the longest dimension is 4.980-4.989 g / cm 3 The maximum pore diameter was measured to be 1.4 um, with a Sa value of 18 nm and a pore size of 1178×10 after the disclosed CF4 / O2 etching process. -5 An Sdr value of 0.65um was measured using the line intercept technique for this sample.
[0308] In another example, sample 353 was prepared as follows: 6.5-7.5 m 2 Yttrium oxide powder having a surface area of 1.5-2.5 m / g and an average of 11 ppm total impurities, corresponding to a powder purity of 99.9989%, was used to form a sintered yttrium oxide body having a longest dimension of 406 mm. Firing of the powder at 1000°C for 24 hours yielded a surface area of 1.5-2.5 m. 2The average mass fraction was 1.0 g / g. Pressure was pre-applied at 5 MPa and the temperature was ramped from room temperature to 800°C at 10°C / min. Simultaneous application of heat and pressure was performed with a heating rate of 10°C / min and a pressure ramp from 800°C to 1000°C to 30 MPa. Pressure was maintained at 30 MPa from 1000°C to the sintering temperature at a heating rate of 10 C / min. Sintering was performed at a temperature of 1475°C and a pressure of 30 MPa for a sintering duration of 60 minutes. Heating and pressing was terminated after the sintering period and natural cooling occurred. The sintered yttrium oxide bodies were annealed in an oxygen-containing environment at 1400°C for 0 minutes (no isothermal annealing time) with a heating rate of 0.8°C / min and a passive cooling rate of 0.8°C / min. The average density of the annealed and sintered yttrium oxide bodies was 4.981 g / cm 3 It was.
[0309] In another example, sample 414 was prepared as follows: 2 Yttrium oxide powder having a surface area of 1.0 μg / g and an average of 11 ppm total impurities, corresponding to a powder purity of 99.9989%, was used to form a sintered yttrium oxide body having a longest dimension of 406 mm. Firing of the powder at 500° C. for 48 hours yielded a surface area of 6.5-7.5 m. 2 The average density of the annealed and sintered yttrium oxide bodies was 1.2 g / g. Pressure was pre-applied at 5 MPa and the temperature was ramped from room temperature to 800°C at 10°C / min. Simultaneous application of heat and pressure was performed with a heating rate of 10°C / min and a pressure ramp of 30 MPa from 800°C to 1000°C. Pressure was maintained at 30 MPa from 1000°C to the sintering temperature with a heating rate of 10°C / min. Sintering was carried out at a temperature of 1400°C and a pressure of 30 MPa for a sintering duration of 60 minutes. Heating and pressing was terminated after the sintering period and natural / passive cooling took place. The average density of the annealed and sintered yttrium oxide bodies was 4.985 g / cm. 3 It was.
[0310] In yet another example, sample 476 was prepared as follows: 2Yttrium oxide powder having a surface area of 1 / g and 5-6 ppm total impurities corresponding to a powder purity of 99.9995% was used to form a sintered yttrium oxide body having a longest dimension of 406 mm. The powder was rolled for 24 hours before sintering without the use of grinding media. Pressure was pre-applied at 5 MPa and the temperature was ramped from room temperature to 600°C at 10°C / min. Simultaneous application of heat and pressure was performed with a heating rate of 5°C / min and a pressure ramp of 30 MPa from 600°C to 1000°C. Pressure was maintained at 30 MPa from 1000°C to the sintering temperature at a heating rate of 5°C / min. Sintering was performed at a temperature of 1475°C and a pressure of 30 MPa for a sintering duration of 60 minutes. Pressure was removed after the sintering time. Cooling was performed using forced convection at 50% blower power. Cooling using various blower power levels allows forced convection cooling rates of 2.5°C / min to 5°C / min. The sintered yttrium oxide bodies were annealed at 1400°C for 4 hours in an oxygen-containing environment using a heating rate of 1°C / min and a cooling rate of 2°C / min. The average density of the annealed and sintered yttrium oxide bodies was 4.953 g / cm 3 and the density range across the longest dimension is 4.891 to 5.014 g / cm 3 It was.
[0311] In one set of examples, samples 084 and 084-1, 085 and 085-1, 086 and 086-1, 087 and 087-1, 095 and 096 were prepared as follows: 100 mm sintered yttrium oxide bodies corresponding to samples 084 and 084-1, 085 and 085-1, 086 and 086-1, 087 and 087-1, 095 and 096 were cut into 6.5-7.5 mm pieces. 2 The powder was prepared from a powder with a surface area of 5–6.5 m / g and an average of 11 ppm total impurities, resulting in a powder purity of 99.9989%. The powder was calcined before sintering at 800 °C for 8 h, yielding a powder purity of 5–6.5 m. 2 The samples had a surface area of 0.1 μm / g. Samples 084-1, 085-1, 086-1, 087-1, 095 and 096 were annealed at 1400° C. for 8 hours at a ramp rate of 5° C. / min in an oxygen environment. The density and process conditions are as disclosed in the corresponding density and sintering / annealing tables herein.
[0312] Comparative Sample 107: The comparative yttrium oxide body was determined to be 99.9958% pure by ICPMS with 42 ppm contaminants. Porosity measurements were performed as disclosed herein and a maximum pore size of 38 um was measured. Particle size measurements were performed and a large average particle size of 27 um was measured. The material had a mass of 4.987 g / cm3 with a standard deviation of 0.038 using the Archimedes method. 3 The material was measured to have an average density of 100 nm. Although the exact sintering conditions are unknown, it is likely that high sintering temperatures in excess of 1600° C. were used for extended periods such as several days to sinter the yttrium oxide powder to form this material. These parameters contribute to the large grain size measured. The sample exhibited significant fractional areas of porosity with large pore sizes and poor etching performance and extensive surface roughness compared to sintered yttrium oxide as disclosed.
[0313] Comparative Sample 108: The material properties of the comparative yttrium oxide body were analyzed. The comparative yttrium oxide body was determined to be 99.8356% pure by ICPMS with 1644 ppm of contaminants including 1291 ppm of zirconia as a sintering aid to promote densification. Porosity measurements were performed as disclosed herein and a maximum pore size of 12 um was measured. The material was determined to have an average density of 4.997 g / cc with a standard deviation of 0.011 using the Archimedes method. While the exact sintering conditions are unknown, it is believed that zirconia may be added to the powder to promote densification and reduce etching performance in order to sinter the yttrium oxide to form this material. The sample showed significant fractional areas of porosity with larger pore sizes and surface roughening compared to sintered yttrium oxide as disclosed.
[0314] Comparative Sample 118: The comparative yttrium oxide body was determined to be 99.9967% pure by ICPMS with 33 ppm contaminants. Porosity measurements were performed as disclosed herein and a maximum pore size of 7 um was measured. The average density was measured to be 5.003 g / cc using the Archimedes method. The sample showed significant fractional areas of porosity with large pore sizes and poor etching performance compared to sintered yttrium oxide as disclosed.
[0315] Tables 4-7 summarize the process conditions and resulting densities of samples prepared according to the process of the present disclosure.
[0316] [Table 4-1]
[0317] [Table 4-2]
[0318] [Table 5]
[0319] [Table 6]
[0320] [Table 7]
[0321] [Table 8]
[0322] Tables 9 and 10 summarize the purities measured for the starting powder and sintered yttrium oxide samples made according to the processes disclosed herein.
[0323] [Table 9-1]
[0324] [Table 9-2]
[0325] Table 10 shows the maintenance of purity during the process disclosed herein from powder to sintered yttrium oxide body.
[0326] [Table 10]
[0327] Tables 11-13 show the etching results of different process gases for quartz (TSC 03), commercial yttrium oxide parts (107, 108, 118), and sintered yttrium oxide samples prepared according to the present disclosure, including the processing conditions. The CF4 / O2 etch was performed in a two-step process. Step 1 was performed at a pressure of 10 mtorr, a CF4 flow rate of 90 sccm, an O2 flow rate of 30 sccm, an argon flow rate of 20 sccm, a bias voltage of 600 V, and a power of 2000 W for 1500 seconds. Step 2 was performed at a pressure of 10 mtorr, a CF4 flow rate of 0 sccm, an O2 flow rate of 100 sccm, an argon flow rate of 20 sccm, a bias voltage of 600 V, and a power of 2000 W for 300 seconds. Steps 1 and 2 were repeated consecutively until the CF4 exposure time for the first step was 24 hours. The O2 etch conditions were: pressure 25 mtorr; CF4 / SF6 flow rate 0 sccm; O2 flow rate 100 sccm; Ar flow rate 20 sccm; bias voltage 600 V. Total 6 hours at power 2000 W and the SF6 etch conditions were: pressure 25 mtorr; SF6 flow rate 100 sccm; O2 flow rate 0 sccm; Ar flow rate 50 sccm; bias voltage 300 V; total 24 hours at power 2000 W. The results show the excellent corrosion resistance of the sintered yttrium oxide bodies made according to the present disclosure.
[0328] Sintered yttrium oxide bodies prepared according to the present development preferably exhibit a step height of 0.2-0.98 μm for the CF4 / O2 etching process disclosed herein, 0.27-0.44 μm for the SF6 etching process disclosed herein, and 0.1-0.13 μm for the O2 etching process disclosed herein.
[0329] The sintered yttrium oxide body prepared according to the present development preferably has a melting point of 0.6×10 for the disclosed CF / O etching process. 5 ~3.4×10 5 μm 3 of etch volume, 0.8×10 for the SF etching process disclosed herein 5 ~1.4×10 5 μm 3 and 0.28-0.39 μm for the O etching process disclosed herein. 3 Shows.
[0330] Sintered yttrium oxide bodies prepared according to the present development preferably exhibit etch rates of 0.14-0.68 nm / min for the CF4 / O2 etching process disclosed herein, 0.19-0.310 nm / min for the SF6 etching process disclosed herein, and 0.07-0.09 nm / min for the O2 etching process disclosed herein.
[0331] [Table 11]
[0332] [Table 12]
[0333] [Table 13]
[0334] [Table 14]
[0335] Grain Boundaries The composition and properties of grain boundaries can be related to etching and erosion performance. As reported in M. Watanabe and DB Williams in "The quantitative analysis of thin film specimens; a review of progress from the Cliff-Lorimer to the new Zeta-factor methods" (J. Microsc. 221 (2006) 89-109), which is incorporated herein by reference in its entirety, grain boundary properties can be calculated by ξj (Zeta) factor quantification. Mass thickness (ρt) and elemental composition (CN) are calculated as follows:
[0336]
number
[0337] where ρ is the specimen density, t is the specimen thickness, the zeta coefficient is for element j with known chemistry and thickness, Ij is the intensity for element j, and De is the electron dose calculated as follows:
[0338]
number
[0339] In use ρt, the X-ray signal can be corrected for absorption according to the following equation:
[0340]
number
[0341]
number
[0342] Mass thickness (ρt) and elemental composition (CN) were then calculated with correction for x-ray signal absorption as reported in "Quantification of boundary segregation in the analytical electron microscope" (M. Watanabe, D.B. Williams, J. Microsc. 221 (2006) 89-109), which is incorporated herein by reference in its entirety. An exemplary procedure for the Zeta factor method is disclosed according to FIG. 32 (Watanabe / Williams 2006).
[0343] Then, EDS (Energy Dispersive X-ray Spectroscopy) spectra were obtained from selected areas on the grain boundary and both adjacent grains, as shown in FIG. 9, and the difference in elemental composition from the EDS spectra between the grain boundary and the bulk grains was determined in atoms / nm. 2 According to Keast et al., it is calculated as the excess coverage at 1000 nm (VJ Keast, DB Williams, J. Microscopy Vol. 199 Pt. 1, (2000) pp. 45-55). 2 The unit excess coverage (or grain boundary coverage) describes the grain boundaries by the following feature Γ, which can be calculated according to the following formula:
[0344]
number
[0345] where ρ is atoms / nm 3 is the density of the matrix in units, Am and As are the atomic masses of the matrix and the segregant, respectively, and the geometric factor V / A is the ratio of the interaction volume to the area of the grain boundaries within the interaction volume, which is a function of d and the total sample thickness. Segregants as used herein include silica.
[0346] A positive number for the excess coverage indicates that the grain boundary has a higher concentration of a particular element relative to the bulk grain, and correspondingly a negative number indicates that the element has a higher concentration in the bulk grain than in the grain boundary.
[0347] A commercial yttrium oxide sample, Comparative Sample 107, was analyzed for its grain boundary composition and excess coverage. Figure 10 shows the atoms / nm across several grain boundaries for Sample 107. 2 The results are shown in units of excess coverage. Silica has approximately 8 atoms / nm2 of coverage over adjacent particles. 2 ~10 atoms / nm 2 was present at the grain boundaries in an excess amount of .
[0348] Sample 114, formed from a common powder supplier as sample 152, was analyzed for its grain boundary composition and excess coverage. 2 Results are shown in units of excess coverage. Silica has approximately 2 atoms / nm2 relative to the bulk particle composition. 2 ~about 4 atoms / nm 2 All other elements were present at excess coverage less than the coverage of silica. These low levels of elements other than yttrium oxide present at the grain boundaries of Sample 114, which corresponds to Sample 152, can provide favorable etching results as reported in Tables 8, 9, and 10 across a variety of process gases.
[0349] Sample 157: Dielectric loss Sample 157 is a sintered yttrium oxide sample having a diameter of 203 mm (8 inches) and a thickness of 5 mm that was sintered at 1550°C for 30 minutes at 10-25°C / min under a pressure of 30 MPa. It was not annealed. The density was >98.5% of the theoretical density of yttrium oxide, reported as 5.03 g / cc. The dielectric results are listed in Table 15.
[0350] [Table 15]
[0351] In addition, the dielectric loss (or dissipation factor) can be affected by the particle size and particle size distribution. Finer particle sizes can also result in reduced dielectric loss, thereby providing reduced heating during use at higher frequencies. -4 ~5.5×10 -2 , preferably 1 x 10 -4 ~5×10 -2 , preferably 1 x 10 -4 ~4×10 -2 , preferably 1.6 x 10 -2 ~5×10 -2 , preferably 1 x 10 -4 ~2×10 -2 A dielectric loss of about 100% can be achieved for sintered ceramic bodies containing high purity yttrium oxide bodies. Yttrium oxide sample 157 has an average dielectric constant of 11.3 and a dielectric loss of 3.6×10 over four measurements, as listed in Table 15. -2 The average dielectric loss was 0.01 to 0.01.
[0352] With reference to the figures, the selection results are summarized as follows: 12 shows the single step CF etch volume of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 compared to sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 according to embodiments of the present disclosure. The sintered yttrium oxide samples according to the present disclosure are significantly more etch resistant than the prior art.
[0353] 13 shows the CF4+O2 average etch volume of prior art TSC 03 (quartz) and sintered yttrium oxide samples 118 and 107 compared to various sintered yttrium oxide samples made according to embodiments of the present disclosure. The sintered yttrium oxide samples according to the present disclosure are significantly more etch resistant than the prior art.
[0354] 14 shows the CF4+O2 average step height for prior art TSC 03 (quartz) and sintered yttrium oxide samples 118 and 107 compared to various sintered yttrium oxide samples made according to embodiments of the present disclosure. The sintered yttrium oxide samples according to the present disclosure are significantly more etch resistant than the prior art.
[0355] 15 shows the average CF4+O2 etch rates of prior art TSC 03 (quartz), sintered yttrium oxide samples 118 and 107 compared to various samples made according to embodiments of the present disclosure. The sintered yttrium oxide samples according to the present disclosure are significantly more etch resistant than the prior art.
[0356] 16 shows 50x SEM micrographs of the surfaces of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 before and after the single-step CF4 etching process. Significant etching is observed.
[0357] 17 shows SEM micrographs at 1000X of the surfaces of sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 made in accordance with the present disclosure before and after a single-step CF4 etching process. The samples made in accordance with the present disclosure are resistant to etching.
[0358] 18 shows SEM micrographs at 1000x of the surfaces of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 before and after the single-step CF4 etching process. Significant etching is observed.
[0359] 19 shows SEM micrographs at 1000X of the surfaces of sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 made in accordance with the present disclosure before and after a single-step CF4 etching process. The samples made in accordance with the present disclosure are resistant to etching.
[0360] Figure 20 shows 5000X SEM micrographs of the surfaces of prior art sintered yttrium oxide samples 107 and 118 before and after the CF4 + O2 etching process. Significant etching is observed.
[0361] 21 shows SEM micrographs at 5000X of the surfaces of sintered yttrium oxide samples 152 and 189-1 made in accordance with the present disclosure before and after a CF4+O2 etching process. The samples made in accordance with the present disclosure are resistant to etching.
[0362] 22 shows SEM micrographs at 1000x and 5000x of the edge and center of a sintered yttrium oxide sample 457 made in accordance with the present disclosure. Uniform density and minimal to no porosity are seen across the entire surface. The sample made in accordance with the present disclosure is dense and resistant to etching.
[0363] FIG. 23 shows that the yttrium oxide bodies (H1 / 66 to H4 / 152) according to one embodiment of the present disclosure do not have pores with a pore size greater than 2.00 μm.
[0364] 24 is a graph showing the developed interfacial area ratio Sdr at 50x optical magnification for prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 compared to sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 according to embodiments of the present disclosure before and after a single-step CF4 etching process. Samples made according to the present disclosure are resistant to etching.
[0365] 25 is a graph showing the arithmetic mean height Sa (nm) at 50x optical magnification of prior art sintered yttrium oxide samples CM1 / 107 and CM2 / 108 compared to sintered yttrium oxide samples H1 / 66, H2 / 65, and H3 / 79 according to embodiments of the present disclosure before and after a single-step CF4 etching process. Figures 21 and 22 show that the yttrium oxide materials according to embodiments of the present invention (H1 / 66-H3 / 79) have significantly lower developed interface area ratios Sdr and arithmetic mean heights Sa compared to the comparative materials (CM1 / 107 and CM2 / 108).
[0366] 26 is a graph showing the developed interfacial area ratio Sdr of various sintered yttrium oxide samples from the examples before and after a CF4+O2 etching process. Samples made according to the present disclosure are resistant to etching.
[0367] 27 is a graph showing the arithmetic mean height Sa (nm) of various samples from the examples before and after the CF4+O2 etching process. Samples made according to the present disclosure are resistant to etching.
[0368] 28 is a graph showing the areal porosity of various sintered yttrium oxide samples from the Examples compared to prior art sintered yttrium oxide samples. The yttrium oxide materials according to one embodiment of the invention (H1 / 66 to H4 / 152) have a much lower pore area percent compared to the comparative materials (CM1 / 107 and CM2 / 108).
[0369] 29 is a graph showing cumulative area (%) versus pore size (pore size distribution) for various samples from the examples compared to prior art sintered yttrium oxide samples. In particular, for pore diameters less than 1 μm, the cumulative percent of area comprised of porosity is 96-100% for yttrium oxide materials H1 / 66-H3 / 79 according to an embodiment of the invention, while for comparative materials CM1 / 107-CM3 and H5 / 62, the cumulative percent of area is about 10% or less.
[0370] 30 is a graph showing the porosity distribution versus log pore size for various samples from the examples compared to prior art sintered yttrium oxide samples. Prior art materials 107, 108, and 118 exhibit larger pore sizes, on the order of 7 um or greater, and a higher percentage of the surface, and therefore volume, of the sintered yttrium oxide body that contains porosity.
[0371] FIG. 31 is a graph showing the sintering pressure and temperature conditions required to obtain a sintered yttrium oxide body having a density of 98% or greater relative to the theoretical density of yttrium oxide.
[0372] Although several embodiments have been described as disclosed herein, it will be understood that various modifications may be made without departing from the spirit and scope of the embodiments disclosed herein. Accordingly, other embodiments are within the scope of the following claims.
Claims
1. Total impurity level of 40 ppm or less, 4.98 g / cm 3 and has a density of 1 atom / nm 2 More than 10 atoms / nm 2 1. A sintered yttrium oxide body having at least one grain boundary containing an over-coverage of silica of at least one surface containing at least one pore, each pore being no greater than 5 μm in diameter.
2. 2. The sintered yttrium oxide body of claim 1, wherein any pore has a diameter of 4 μm or less.
3. 3. The sintered yttrium oxide body of claim 1 or 2, wherein the total impurity level is 35 ppm or less.
4. 4. The sintered yttrium oxide body of claim 1, having a pore size distribution with a maximum pore size of 1.50 μm for 95% or more of all pores on the at least one surface.
5. 5. The sintered yttrium oxide body of claim 1, wherein the at least one surface has an area that is less than 0.15% occupied by pores.
6. 6. The sintered yttrium oxide body of any one of claims 1 to 5, having at least one dimension between 100 mm and 600 mm.
7. 7. The sintered yttrium oxide body of claim 6, wherein the density does not vary by more than 3% along the at least one dimension.
8. 1. A process for making a sintered yttrium oxide body, comprising: a. placing yttrium oxide powder within an interior volume defined by a spark plasma sintering tool, the spark plasma sintering tool comprising a die including a sidewall including an inner wall having a diameter defining the interior volume, and an outer wall; an upper punch and a lower punch operatively connected to the die, each of the upper punch and the lower punch having an outer diameter smaller than a diameter of the inner wall of the die, thereby creating a gap between each of the upper punch and the lower punch and the inner wall of the die when at least one of the upper punch and the lower punch is moved within the internal volume of the die, the gap being between 10 μm and 70 μm in width, and creating a vacuum condition within the internal volume; b. applying a pressure of 10 MPa to 60 MPa to the yttrium oxide powder by moving at least one of the upper punch and the lower punch within the internal volume of the die to apply pressure to the yttrium oxide powder while heating to a sintering temperature of 1200-1600°C to form a sintered yttrium oxide body; c. Reducing the temperature of the sintered yttrium oxide body, wherein the yttrium oxide powder of step a) is cooled to 100° C. 2 / g or less, and the sintered yttrium oxide body has a total impurity level of 40 ppm or less, a surface area of 4.98 g / cm 3 or greater, at least one surface containing at least one pore, each pore having a diameter of 5 μm or less; The process includes:
9. The process of claim 8, further comprising the step of annealing the sintered yttrium oxide body by increasing the temperature of the sintered yttrium oxide body to an annealing temperature and performing annealing.
10. The process of claim 9, further comprising the step of: e. reducing the temperature of the annealed sintered yttrium oxide body to ambient temperature by removing the heat source applied to the sintered yttrium oxide body.
11. The process of claim 9 or 10, further comprising: machining the annealed sintered yttrium oxide body to produce a sintered yttrium oxide body component, the component being selected from the group consisting of a dielectric or RF window, a focus ring, a nozzle or gas injector, a showerhead, a gas distribution plate, an etch chamber liner, a plasma source adaptor, a gas inlet adaptor, a diffuser, an electronic wafer chuck, a chuck, a puck, a mixing manifold, an ion suppressor element, a faceplate, an isolator, a spacer, and a guard ring.
12. The process according to any one of claims 8 to 11, wherein the yttrium oxide powder is calcined prior to step a).
13. The yttrium oxide powder has a thickness of 1.5 to 7.0 m 2 The process of any one of claims 8 to 12, wherein the surface area is 0.1 - 1.0 g.
14. The process according to any one of claims 8 to 13, wherein the sintering is carried out for a time period between 1 minute and 120 minutes.
15. The process of any one of claims 8 to 14, wherein any pore on said at least one surface has a diameter of 4 μm or less.
16. 16. The process of any one of claims 8 to 15, wherein the total impurity level of the sintered yttrium oxide body is 35 ppm or less.
17. The process of any one of claims 8 to 16, wherein the sintered yttrium oxide body has at least one dimension between 100 mm and 600 mm.
Citation Information
Patent Citations
Light transmitting sintered material of yttria and production thereof
JP1992074764A
Light transmitting ceramic and method for producing the same
JP2002326862A
Method for manufacturing oxide-based dielectric ceramic sintered compact and oxide-based dielectric ceramic sintered compact
JP2004026616A
Yttria ceramic component for use in plasma treatment device and its manufacturing method
JP2006021990A
Y2o3-based sintered compact
JP2008260651A