Resin films, laminates, display components, and healthcare sensors
A resin film with controlled properties and urethane bonds addresses the issues of flexibility, restorability, and appearance quality in displays and sensors, maintaining concealment by optimizing pigment dispersibility and crosslinking.
Patent Information
- Application Number
- JP2020055824
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-26
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2040-03-26
AI Technical Summary
Existing resin films used in displays and sensors lack sufficient flexibility, restorability, and appearance quality while maintaining concealment properties, as they often form aggregates and impair elasticity due to insufficient pigment dispersibility and cohesive forces.
A resin film with a specific structure and urethane bond, containing a colorant, with controlled light transmittance, storage modulus, loss tangent, and pigment distribution, which minimizes physical crosslinks and enhances chemical crosslinking to maintain flexibility and appearance quality.
The resin film achieves concealment without impairing elasticity or appearance quality, ensuring high flexibility, restorability, and improved pigment dispersibility, preventing aggregates and defects.
Smart Images

Figure 0007567188000013 
Figure 0007567188000014 
Figure 0007567188000015
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin film, a laminate, a display member, and a healthcare sensor that combine stretchability, quality, and hiding power. [Background technology]
[0002] With the current development of the IoT society, small devices that can be freely transformed are being developed. For example, foldable and rollable displays are being put to practical use in smartphones and tablets. In addition, wearable sensors that can bend and stretch have been proposed to follow the curves and movements of the body, and it is expected that the use of these devices will lead to the development of new applications.
[0003] On the other hand, when using these devices, they require a certain degree of concealment, i.e., the material underneath cannot be seen through. For example, in displays, resin films with concealment properties are required to prevent reflected light from interfering with the light emitted by the OLED (organic light-emitting diode) embedded in the device, and in wearable sensors, resin films with concealment properties are required to prevent the embedded wiring from being seen.
[0004] As a representative example of such a resin film resin, there is proposed an "ultraviolet-curable resin composition capable of giving a cured product having excellent resin film adhesion, flexibility, and insulating properties, low transmittance, and excellent hiding power" as described in Patent Document 1.
[0005] Furthermore, as an example of a composition having excellent flexibility, a "black photosensitive composition exhibiting sufficient hiding power" has been proposed in Patent Document 2.
[0006] As an example of a film with excellent restoring properties, Patent Document 3 proposes a "dry resist film capable of forming a cover coat layer using a black colorant, which has high light-blocking properties while also having excellent patterning properties that allow for the formation of fine openings, which is in demand in recent years, and which also satisfies thermocompression resistance, migration resistance, and flexibility." [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2013-194156 A [Patent Document 2] JP 2012-141605 A [Patent Document 3] JP 2018-152606 A Summary of the Invention [Problem to be solved by the invention]
[0008] Resin films with opacity used in the aforementioned displays and sensors are required to have the opacity without impairing their "free bending and stretching." For "free bending and stretching," it is now required that they be able to be stretched greatly with a small force and almost completely restored at a temperature of 0°C or lower, and at a fast cycle of more than once per second. In other words, even when a colorant is added to the resin composition to impart opacity, it is now required that the flexibility and restorability of the resin itself is not impair.
[0009] In addition, in displays and sensors, this resin film is used in a laminated state by bonding it to other parts, so that the resin film is required to have high appearance quality so that the unevenness and color difference of the resin film do not appear on the laminate surface. In order to obtain high appearance quality of the resin film, it is also required to prevent the colorant from becoming aggregates and causing repelling and defects in the resin film. In other words, for these applications, a resin film that has flexibility, recovery, and appearance quality while being given concealment properties is required.
[0010] In response to the above demands, the present inventors have confirmed the above viewpoints and found that the material proposed in Patent Document 1 is indeed excellent in hiding power, but is insufficient in flexibility and restorability.
[0011] Furthermore, the material proposed in Patent Document 2 has excellent flexibility, but is insufficient in quality and restorability.
[0012] In addition, the material proposed in Patent Document 3 has excellent recovery and a certain degree of flexibility, but these are not at the level required for this application, and the appearance quality is also insufficient.
[0013] In view of the above, an object of the present invention is to provide a resin film or laminate that has been imparted with concealing properties without impairing stretchability or appearance quality, and a display member or healthcare sensor that is excellent in quality. [Means for solving the problem]
[0014] In order to solve the above problems, the present inventors have conducted extensive research and have completed the following invention. (1) A resin film containing a structure of Chemical Formula 1 and a urethane bond, and satisfying all of the following conditions 1 to 4:
[0015] [ka]
[0016] In addition, R in Chemical Formula 1 1 refers to a hydrogen or a methyl group.
[0017] Condition 1: The resin film contains a colorant.
[0018] Condition 2: The total light transmittance of the resin film, measured by the method specified in JIS K7375 (2008), is 2% or more and 20% or less.
[0019] Condition 3: The storage modulus of the resin film at a temperature of 25°C and a frequency of 1 Hz is 0.5 MPa or more and 50 MPa or less.
[0020] Condition 4: The loss tangent of the resin film at 25°C is 0.5 or less. (2) The resin film according to (1), which contains a pigment and satisfies condition 5.
[0021] Condition 5: The pigment occupies an area of the cross section of the resin film of 0.1% or more and 2.0% or less. (3) A resin film according to (1) or (2), which contains a pigment and satisfies the following condition 6.
[0022] Condition 6: The 95% particle size (D 95 ) and 50% particle size (D 50 ) and F A The ratio of the average value of D95 and D50 of the pigment in the area from the surface to 0% to 30% and 70% to 100% of the thickness direction is F. B Then, equations 1 and 2 are satisfied.
[0023] Formula 1:F A <2.4 Formula 2:|F A -F B |<0.4 (4) The resin film according to any one of (1) to (3), wherein the pigment is a black pigment. (5) The resin film according to (4), which satisfies condition 7.
[0024] Condition 7: The absorption coefficient of the resin film (ε A ) satisfies Equation 3.
[0025] Equation 3: ε A (1 / μm)=100×(Log 10 100 / T) / (A×d)>2.0 Here, A is the occupied area ratio (%) of the black pigment, d is the thickness (μm) of the resin film, and T is the total light transmittance (%) of the resin film. (6) A laminate having a supporting substrate on at least one surface of the resin film according to any one of (1) to (5), wherein the peel strength between the supporting substrate and the resin film is 1 N / 50 mm or less. (7) A display member comprising the resin film according to any one of (1) to (5). (8) A healthcare sensor comprising the resin film according to any one of (1) to (5). Effect of the Invention
[0026] It is possible to provide resin films and laminates with concealing properties without compromising stretchability or appearance quality, as well as high-quality display components and healthcare sensors. [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Diagram 2] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Diagram 3] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 4] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Diagram 5] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 6] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 7] FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. [Figure 8]FIG. 1 is a cross-sectional view showing an example of a laminate according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] Before describing the modes for carrying out the present invention, the present inventors consider the following reasons why the problems faced by the present invention cannot be solved by the conventional techniques.
[0029] First, let us consider the characteristics of the material. Colorants can be mainly divided into pigments and dyes from the viewpoint of solubility. Dyes do not have high weather resistance or stability over time of hiding power compared to pigments, and may be limited to applications where these are not a problem. On the other hand, pigments do not dissolve in coating materials, so they tend to form aggregates, but they have high weather resistance and high stability over time of hiding power. Therefore, when using pigments, it is necessary to increase dispersibility. In addition, when dispersing a pigment in a resin precursor, it is preferable that the skeleton of the resin precursor has functional groups that interact with the pigment all over the surface. If the functional groups that interact with the pigment gather locally, the pigment also gathers locally, resulting in the formation of aggregates. Here, carbon black, which is a common pigment, can form two types of interactions: π-π interactions derived from the carbon black skeleton and hydrogen bonds derived from hydroxyl groups or carbonyl groups on the carbon black surface. Therefore, when using carbon black as a pigment, it is considered that it is preferable to use a skeleton of the resin precursor that has an aromatic ring or a functional group with high hydrogen bonding properties and can be efficiently dispersed in order to prevent the pigment from aggregating. On the other hand, when these functional groups gather together, they form hard segments, and the cohesive force of these segments creates recovery. In other words, there is a trade-off between the dispersibility and recovery of the pigment, and in order to resolve this, it is thought that efficient dispersion and the formation of crosslinking points are necessary.
[0030] The material described in Patent Document 1 uses bisphenol A type epoxy acrylate with a number average molecular weight of 6000 or less as a resin precursor, and carbon black as a colorant. Because a resin precursor with a relatively low molecular weight is used, the degree of freedom of the resin itself is low, and accumulation of phenol moieties due to π-π interactions is unlikely to occur, and therefore aggregation of carbon black is unlikely to occur.
[0031] On the other hand, because the molecular weight of the resin precursor is low, the degree of freedom of the soft segments that do not have cohesive strength is also low, resulting in insufficient flexibility.In addition, as for the restorability, because the degree of freedom of the resin precursor is low, it is difficult to form interactions between the phenolic moieties, and because the frequency of contact with the acrylic group is low, UV curing is not sufficient, and the level required for this application is not reached.
[0032] The material described in Patent Document 2 uses, as a resin precursor, a combination of bisphenol A type epoxy acrylate and urethane acrylate, each having a number average molecular weight of 5,000 or more and 20,000 or less.
[0033] Compared to the one in Patent Document 1, the molecular weight is high and therefore the flexibility is high, but the degree of freedom of the resin precursor itself is high, so that the soft segment and the hard segment are likely to form a microphase separation structure, and the carbon black gathers due to the cohesive force between the hard segments to form aggregates, resulting in insufficient appearance quality. In addition, because the carbon black aggregates, the carbon black content required to impart high hiding power is high, the specific surface area of the carbon black in the resin film is high, and the curing by active energy rays is insufficient, resulting in insufficient recovery.
[0034] The material described in Patent Document 3 uses bisphenol A type epoxy acrylate with a number average molecular weight of 7000 or more and 25000 or less as a resin precursor, and further adds a low molecular weight isocyanate as a heat curing agent to enhance the restorability. Compared to the material described in Patent Document 1, the material has a high molecular weight and thus a certain degree of flexibility, but as hard segments, physical crosslinking due to π-π interactions of the phenol moiety, chemical crosslinking due to UV curing, and chemical crosslinking due to heat curing are formed, and the cohesive force is high, so ultimately the flexibility is insufficient for this application. In addition, the hydroxyl group and isocyanate, which are the source of the heat curing reaction, form hydrogen bonds with titanium black, which makes titanium black more likely to aggregate and deteriorates the appearance quality.
[0035] In response to this, the present inventors came up with the idea of solving the above-mentioned problems by reducing the cohesive force due to physical crosslinks such as π-π interactions and hydrogen bonds possessed by the resin precursor to the minimum necessary, by making the functional groups that form these interactions exist evenly throughout the resin film composition, thereby increasing the dispersibility of the colorant that interacts with these functional groups, and by forming small and strong chemical crosslinks at a low density by UV curing, thereby imparting hiding power without impairing stretchability or appearance quality, and after extensive investigations, arrived at the present invention. The present invention will be described in detail below.
[0036] It is important that the resin film of the present invention contains the structure of Chemical Formula 1 and a urethane bond and satisfies all of the following conditions 1 to 4.
[0037] [ka]
[0038] In addition, R in Chemical Formula 1 1 refers to a hydrogen or a methyl group.
[0039] Condition 1: The resin film contains a colorant.
[0040] Condition 2: The total light transmittance of the resin film, measured by the method specified in JIS K7375 (2008), is 2% or more and 20% or less.
[0041] Condition 3: The storage modulus of the resin film at a temperature of 25°C and a frequency of 1 Hz is 0.5 MPa or more and 50 MPa or less.
[0042] Condition 4: The loss tangent of the resin film at 25°C is 0.5 or less.
[0043] Whether the resin film contains the above-mentioned structure or bond can be determined by various analytical methods, but methods using FT-ATR-IR (Fourier transform infrared spectroscopy) or pyrolysis GC-MS (gas chromatography mass spectrometry) are convenient. It can also be determined from the raw materials that form the resin film.
[0044] When the resin film has the above-mentioned structure and bond, crosslinks can be formed and the film can be endowed with restoring properties. Furthermore, the presence of crosslinks allows urethane bonds, which are highly polar and exhibit affinity with colorants, to be present evenly without aggregation.
[0045] More preferably, the structure of Chemical Formula 1 includes the structure of Chemical Formula 2.
[0046] [ka]
[0047] In addition, R in Chemical Formula 2 1 refers to a hydrogen or a methyl group.
[0048] R in Chemical Formula 2 2 refers to one of the following: - a substituted or unsubstituted alkylene group, - a substituted or unsubstituted arylene group, An alkylene group having an internal ether group, ester group, or amide group, Arylene groups having an internal ether group, ester group, or amide group, - Unsubstituted alkylene groups having an internal ether group, ester group, or amide group; An unsubstituted arylene group having an internal ether group, ester group, or amide group.
[0049] The segment formed by the urethane bond preferably includes a structure represented by Chemical Formula 3.
[0050] [ka]
[0051] In addition, R in Chemical Formula 3 3 refers to one of the following: - a substituted or unsubstituted alkylene group, Substituted or unsubstituted arylene groups.
[0052] It is important that the resin film of the present invention contains a colorant.
[0053] The presence of colorants in resin films can be determined by various analytical methods, but the easiest method is to use cross-sectional SEM (scanning electron microscope) and TOF-SIMS (time-of-flight secondary ion mass spectrometry) of the film. The measurement method will be described later.
[0054] By including a colorant in the resin film, the resin film can be colored and can be provided with hiding properties.
[0055] It is important that the resin film of the present invention has a total light transmittance of 2% or more and 20% or less as specified in JIS K7375 (2008).
[0056] By setting the total light transmittance of the resin film to 2% or more and 20% or less, the film has sufficient concealing properties and can suppress poor curing caused by UV irradiation. From the same viewpoint, the total light transmittance of the resin film is preferably set to 5% or more and 10% or less.
[0057] The total light transmittance is a value measured by a haze meter, and the measuring method will be described later.
[0058] It is important that the resin film of the present invention has a storage modulus of 0.5 MPa or more and 50 MPa or less under conditions of a temperature of 25° C. and a frequency of 1 Hz. By having a storage modulus of 0.5 MPa or more, it is possible to prevent the resin film from being too tacky and difficult to handle, and by having a storage modulus of 50 MPa or less, it is possible to make the resin film easily deformable. From the same viewpoint, it is preferably 1.0 MPa or more and 25 MPa or less, and more preferably 3.0 MPa or more and 10 MPa or less.
[0059] It is important that the resin film of the present invention has a loss tangent at 25° C. of 0.5 or less.
[0060] By setting the loss tangent to 0.5 or less, sufficient restorability can be obtained when used as a resin film. From the same viewpoint, the loss tangent of the resin film at 25° C. is preferably 0.2 or less, and more preferably 0.05 or less.
[0061] The storage modulus and loss tangent refer to values measured by DMA (dynamic mechanical analysis) method, and the measurement method will be described later.
[0062] By satisfying the above conditions 3 and 4, it is possible to achieve both elasticity and recovery. The mechanism is assumed to be that the physical crosslinking that occurs between the resin precursors is suppressed to the minimum necessary, recovery is achieved based on chemical crosslinking, and the inherent elasticity of the high molecular weight resin precursor is maintained. Furthermore, by simultaneously satisfying conditions 1 and 2, it is possible to impart hiding power without compromising elasticity and appearance quality. The mechanism is assumed to be that the colorant is dispersed and does not aggregate at the physical crosslinking sites of the resin precursor, and then hiding power can be imparted.
[0063] It is preferable that the resin film of the present invention contains a pigment and satisfies condition 5.
[0064] Condition 5: The pigment occupies an area of the cross section of the resin film of 0.1% or more and 2.0% or less.
[0065] The occupied area ratio of the pigment in the cross section of the resin film can be calculated by analyzing an SEM image of the cross section of the film, and the method for this will be described later.
[0066] Regarding the occupied area ratio, a small occupied area ratio means that the content of the colorant in the resin film is small. By making the occupied area ratio 2.0% or less, the content of the pigment in the resin film is small, and the formation of coarse particles can be suppressed, and by making it 0.1% or more, the weather resistance is high, and the hiding power can be stably maintained even under a humid and hot environment. From the same viewpoint, it is more preferable that the occupied area ratio of the pigment in the cross section of the resin film is 0.2% or more and 1.0% or less.
[0067] It is preferable that the resin film of the present invention contains a pigment and satisfies condition 6.
[0068] Condition 6: The 95% particle size (D 95 ) and 50% particle size (D 50 ) and F A , D of the pigment in the area of 0% to 30% and 70% to 100% of the thickness direction from the surface 95 and D 50 The ratio of F B Then, equations 1 and 2 are satisfied.
[0069] Formula 1:F A <2.4 Formula 2:|F A -F B |<0.4 The particle size of the pigment contained in the resin film can be calculated by analyzing an SEM image of the cross section of the film, and the method for doing so will be described later.
[0070] Here, F in Eq. Ais a parameter indicating the spread of particle size distribution on the inner side of the film, and this value is preferably smaller than 2.4, and more preferably smaller than 2.2.
[0071] F in Eq. A To reduce F to less than 2.4, for example, the ratio of coarse particles can be reduced, i.e., F in Eq. A By making it smaller than 2.4, it is possible to suppress streaks and repelling during production of the resin film.
[0072] The left side of formula 2 is a parameter indicating the difference in the spread of the particle size distribution between the inner side and the surface side of the film, and this value is preferably smaller than 0.4, and more preferably smaller than 0.3.
[0073] The value of the left side of the formula 2 being smaller than 0.4 means that the difference in the spread of the particle size distribution in the thickness direction is small, and the value of the left side of the formula 2 being smaller than 0.4 can be achieved, for example, by increasing the stability of the particles. In other words, by making the value of the left side of the formula 2 smaller than 0.4, the formation of coarse particles can be suppressed, and streaks and repelling can be suppressed when producing a resin film.
[0074] In the resin film of the present invention, the pigment is preferably a black pigment. Black pigments include carbon compounds such as carbon black, graphite, fullerene, carbon fiber, and carbon nanotubes (CNT), and inorganic oxides such as titanium black, aniline black, perylene black, manganese oxide, ferrous oxide, cupric oxide, cobalt oxide, bismuth oxide, chromium oxide, and magnetite. In addition, when the black pigment exceeds 50% by mass with respect to the total amount of pigments contained, a pigment other than black can be used in combination. By making the black pigment 50% by mass or more, the efficiency of imparting the hiding property of the film can be increased.
[0075] The resin film of the present invention preferably satisfies condition 7.
[0076] Condition 7: The absorption coefficient of the resin film (ε A ) satisfies Equation 3.
[0077] Equation 3: ε A (1 / μm)=100×(Log 10 100 / T) / (A×d)>2.0 Here, A is the occupied area ratio (%) of the black pigment, d is the thickness (μm) of the resin film, and T is the total light transmittance (%) of the resin film.
[0078] Here, the extinction coefficient (ε A ) is a parameter that indicates the efficiency of the pigment in imparting hiding power, and in order to make this value greater than 2.0, for example, it can be achieved by appropriately adjusting the type of colorant, the type of resin precursor, and the manufacturing method of the resin film, thereby reducing the pigment content and making the total light transmittance small. A By making the value of the pigment content larger than 2.0, it is possible to ensure the hiding power with a small pigment content, and it is possible to obtain a resin film having excellent hiding power and quality. From the same viewpoint, it is more preferable that the value of the pigment content is larger than 4.0.
[0079] Furthermore, the laminate of the present invention is a laminate having a supporting substrate on at least one surface of the resin film, and the peel strength between the supporting substrate and the resin film is preferably 1 N / 50 mm or less, an example of which is shown in FIG.
[0080] Here, the supporting substrate is an article that is flat in the in-plane direction and on whose surface a resin film-forming coating composition can be spread by the resin film manufacturing method described below when a resin film is provided on one side of the laminate of the present invention.
[0081] The reason for providing a supporting substrate in the laminate of the present invention is that in the manufacturing method of the resin film described later, a liquid coating composition is applied to the supporting substrate and crosslinked to form a resin film, and also to ensure processability and transportability in the post-process in which the resin film is processed. Therefore, as long as it can be peeled from the resin film (preferably with a peeling force of 1 N / 50 mm or less from the resin film) and does not affect the functions including the post-processability of the resin film, it is preferable that the laminate 4 has a supporting substrate 7 including a release layer 6 between it and the resin film 5 as shown in FIG. 2, although there are no particular limitations thereon.
[0082] Furthermore, when the laminate is wound into a roll to produce an intermediate product, in order to stabilize the rolled appearance, the laminate 8 may have a support substrate 11 including a release layer 10 on the side opposite to the resin film 9 as shown in Fig. 3. Of course, the laminate 12 may have a release layer 14 between the resin film 13 and a support substrate 16 including a release layer 15 on the opposite side as shown in Fig. 4. In this case, the release layers 14 and 15 may be the same, but are preferably different because it is necessary to adjust the peeling force between the resin film 9 and the release layer 15 when the laminate is unwound from the roll, and the peeling force between the resin film 13 and the release layer 14 in a later process.
[0083] In order to improve the transportability of the resin film in the process and prevent scratches, the laminate 17 may have a peelable support substrate 19 on one side of the resin film 18 and a peelable protective material on the other side as shown in FIG. 5. The protective material and the support substrate may be the same, but the laminate 21 may have a support substrate 24 including a release layer 23 between the resin film 22 and a protective material 25 as shown in FIG. 6, the laminate 26 may have a support substrate 29 including a release layer 28 between the resin film 27 and a protective material 31 including a release layer 30 as shown in FIG. 7, and the laminate 32 may have a support substrate 35 including a release layer 34 between the resin film 33 and a protective material 37 including an adhesive layer 36 as shown in FIG. 8. Whether the laminate has a protective material having an adhesive layer or a protective material using a release layer is appropriately selected based on the suitability of the subsequent process and the physical properties of the resin film.
[0084] As described above, in the laminate of the present invention, the peel strength between the support substrate and the resin film is 1 N / 50 mm or less, and preferably 800 mN / 50 mm or less. There is no particular lower limit to the peel strength between the support substrate and the resin film, but if it is less than 10 mN / 50 mm, the support substrate and the resin film may peel off or float during the manufacturing process, so the peel strength between the support substrate and the resin film is preferably 10 mN / 50 mm or more.
[0085] The method for measuring the peel strength between the supporting substrate and the resin film will be described later.
[0086] Furthermore, the display member of the present invention preferably contains the resin film. Also, the healthcare sensor of the present invention preferably contains the resin film. By adopting such an embodiment, a high-quality display member or healthcare sensor with little color unevenness can be obtained.
[0087] Here, the display component refers to electronic devices that display images, such as televisions, smartphones, and personal computers, as well as electronic devices that simultaneously have an input function when touched, such as a touch panel, and devices that use them.
[0088] In addition to electronic devices such as the display components mentioned above, healthcare sensors also refer to sensors and devices that use these sensors and sensors that are attached directly to the living body to continuously record biometric information such as respiratory rate, heart rate, body temperature, blood pressure, electrocardiograms, and brain waves, with the aim of maintaining health and improving the quality of medical care.
[0089] [Mode of the present invention] Hereinafter, the embodiment of the present invention will be described in detail.
[0090] [Resin film] The resin film of the present invention is not particularly limited in the number of layers, as long as it has a film-like structure by itself, and may be formed from one layer or two or more layers. Here, the layer refers to a part that has a boundary surface that can be distinguished from adjacent parts in the thickness direction and has a finite thickness. More specifically, when the cross section of the resin film is observed with an electron microscope (transmission type, scanning type) or an optical microscope, it refers to a part that can be distinguished by the presence or absence of a discontinuous boundary surface. Even if the composition changes in the thickness direction of the resin film, if there is no boundary surface between them, it is treated as one layer.
[0091] The resin film of the present invention may have other functions such as gloss, fingerprint resistance, moldability, designability, scratch resistance, antifouling, solvent resistance, antireflection, antistatic, electrical conductivity, heat ray reflection, near infrared absorption, electromagnetic wave shielding, easy adhesion, etc., in addition to the objectives of flexibility, recovery, concealment, and appearance quality, and in this case, one or more layers may be further formed. For example, a functional layer having the above-mentioned functions, an adhesive layer, an electronic circuit layer, a printing layer, an optical adjustment layer, or other functional layers may be provided.
[0092] In addition, when the resin film of the present invention has a multilayer structure, with regard to the above-mentioned condition 6, equations 1 and 2 of condition 6 are calculated for each layer of the resin film having a pigment, and the resin film is deemed to satisfy condition 6 if at least one or more layers having a pigment satisfy equations 1 and 2 of condition 6.
[0093] The thickness of the resin film is not particularly limited and is appropriately selected depending on the application. The lower limit of the thickness of the resin film is not generally determined because it is affected by the elastic modulus, breaking elongation, peeling force and peeling angle between the support substrate and the resin film, etc., but when the same physical properties as those of a general flexible material are realized using the manufacturing method of the laminate described later, the lower limit is about several μm.
[0094] [Laminate] The laminate of the present invention is preferably a laminate having a supporting substrate on at least one side of a resin film exhibiting the above-mentioned physical properties, and the peel strength between the supporting substrate and the resin film is 1 N / 50 mm or less. As long as it is in this form, the laminate may be in a flat state or may have a three-dimensional shape after molding.
[0095] [Supporting base material] The supporting substrate used in the laminate of the present invention may be either a thermoplastic resin or a thermosetting resin, and may be a homogeneous resin, a copolymer, or a blend of two or more kinds. The resin constituting the supporting substrate is preferably one having good moldability, and from this point of view, a thermoplastic resin is more preferable.
[0096] Examples of thermoplastic resins that can be suitably used for the supporting substrate include polyolefin resins such as polyethylene, polypropylene, polystyrene, and polymethylpentene, alicyclic polyolefin resins, polyamide resins such as nylon 6 and nylon 66, aramid resins, polyimide resins, polyester resins, polycarbonate resins, polyarylate resins, polyacetal resins, polyphenylene sulfide resins, fluororesins such as tetrafluoroethylene resin, trifluoroethylene resin, trifluorochloroethylene resin, tetrafluoroethylene-hexafluoropropylene copolymer, and vinylidene fluoride resin, acrylic resins, methacrylic resins, polyacetal resins, polyglycolic acid resins, and polylactic acid resins.
[0097] Examples of thermosetting resins suitable for use in the support substrate include phenol resin, epoxy resin, urea resin, melamine resin, unsaturated polyester resin, polyurethane resin, polyimide resin, silicone resin, etc. The thermoplastic resin is preferably a resin having sufficient stretchability and conformability. From the viewpoints of strength, heat resistance, and transparency, the thermoplastic resin is more preferably a polyester resin, a polycarbonate resin, an acrylic resin, or a methacrylic resin.
[0098] The polyester resin preferably used for the support substrate is a general term for polymers having an ester bond as the main bond in the main chain, and is obtained by polycondensation of an acid component and its ester with a diol component. Specific examples include polyethylene terephthalate, polypropylene terephthalate, polyethylene-2,6-naphthalate, and polybutylene terephthalate. These may also be copolymerized with other dicarboxylic acids and their esters or diol components as the acid component or diol component. Among these, polyethylene terephthalate and polyethylene-2,6-naphthalate are particularly preferred in terms of transparency, dimensional stability, heat resistance, and the like.
[0099] In addition, the supporting substrate may contain various additives, such as an antioxidant, an antistatic agent, a crystal nucleating agent, inorganic particles, organic particles, a viscosity reducer, a heat stabilizer, a lubricant, an infrared absorber, an ultraviolet absorber, and a dopant for adjusting the refractive index.
[0100] Furthermore, the supporting substrate may have either a single layer structure or a laminate structure.
[0101] In addition, a functional layer such as an easy-adhesion layer, an antistatic layer, an undercoat layer, an ultraviolet absorbing layer, or a release layer may be provided in advance on the surface of the supporting substrate in addition to the resin film of the present invention, and the laminate of the present invention preferably has a release layer in order to reduce the peeling force between the supporting substrate and the resin film. The details of the release layer will be described later.
[0102] Examples of supporting substrates provided with a release layer include "Therapeel" (registered trademark) manufactured by Toray Advanced Film Co., Ltd., "Unipeel" (registered trademark) manufactured by Unitika Ltd., "Panapeel" (registered trademark) manufactured by Panac Corporation, "Toyobo Ester" (registered trademark) manufactured by Toyobo Co., Ltd., and "Purex" (registered trademark) manufactured by Teijin Limited, and these products can also be used.
[0103] The surface of the supporting substrate may be subjected to various surface treatments before forming the resin film. Examples of the surface treatments include chemical treatment, mechanical treatment, corona discharge treatment, flame treatment, ultraviolet irradiation treatment, high frequency treatment, glow discharge treatment, active plasma treatment, laser treatment, mixed acid treatment, and ozone oxidation treatment. Among these, glow discharge treatment, ultraviolet irradiation treatment, corona discharge treatment, and flame treatment are preferred, and glow discharge treatment and ultraviolet treatment are more preferred.
[0104] [Release layer] The support substrate used in the laminate of the present invention preferably has a release layer as described above. A support substrate having a release layer is also called a release film. The release layer may be composed of multiple layers from the viewpoint of imparting adhesion, antistatic properties, solvent resistance, etc., and may be present on both sides of the support substrate.
[0105] The composition and thickness of the release layer are not particularly limited as long as the peel strength from the resin film can be within the preferred range described above. From the viewpoints of the in-plane uniformity of the release layer, appearance quality, and peel strength, however, it is preferably 10 to 500 nm, and more preferably 20 to 300 nm.
[0106] [Protective material] The laminate of the present invention may have a protective material on the surface of the resin film opposite to the supporting substrate as shown in FIG. 5. The protective material and the supporting substrate are distinguished in that, in the manufacturing method of the laminate, the one to which the coating composition is applied is the supporting substrate, and the one to which the resin film is laminated after formation is the protective material. The protective material may be the same as or different from the supporting substrate described above, but it is preferable that the protective material has a different peeling force from the supporting substrate described above when used in a later process. The magnitude relationship between the peeling force of the protective material and the supporting substrate from the resin film is appropriately selected depending on the method of use in the later process. Therefore, the protective material may have a release layer as shown in FIG. 7 described above, may have an adhesive layer as shown in FIG. 8, or may not have a layer as shown in FIG. 6.
[0107] [Manufacturing method of resin film] Although the method for producing the resin film of the present invention is not particularly limited, it is preferable to apply a coating composition containing a resin precursor containing a segment of chemical formula 3 or 4 onto a supporting substrate to form a coating layer (step 1), then remove the solvent from the coating layer and dry it (step 2), irradiate with active energy rays to crosslink the resin precursor (step 3) to produce a laminate, and then peel off the supporting substrate from the laminate (step 4).
[0108] The method of applying the coating composition onto the supporting substrate in step 1 is not particularly limited as long as the coating composition can be applied onto the supporting substrate to form a uniform coating layer in the plane. The coating method onto the film can be appropriately selected from a dip coating method, a roller coating method, a wire bar coating method, a gravure coating method, a die coating method (US Pat. No. 2,681,294), and the like. Here, the coating layer refers to a "liquid layer" formed by the coating step.
[0109] The method for removing the solvent in step 2, i.e., the drying method, is not particularly limited as long as it can remove the solvent from the coating layer formed on the support substrate. Drying methods include heat transfer drying (contact with a high-heat object), convection heat transfer (hot air), radiation heat transfer (infrared rays), and others (microwaves, induction heating), and among these, in the manufacturing method of the present invention, a method using convection heat transfer or radiation heat transfer is preferred because it is necessary to precisely make the drying speed uniform even in the width direction.
[0110] The crosslinking method in step 3 involves irradiating the coating layer from which the solvent has been removed after drying with active energy rays to cause a reaction and crosslink the coating film.
[0111] Crosslinking by active energy rays is preferably performed using electron beams (EB) and / or ultraviolet rays (UV) from the viewpoint of versatility. Examples of the type of ultraviolet lamp used for irradiating ultraviolet rays include discharge lamp type, flash type, laser type, and electrodeless lamp type. When ultraviolet curing is performed using a high-pressure mercury lamp, which is a discharge lamp type, the illuminance of the ultraviolet rays is 100 to 3,000 (mW / cm 2), and more preferably 200 to 2,000 (mW / cm 2 ), and more preferably 300 to 1,500 (mW / cm 2 ), and the integrated amount of ultraviolet light is 100 to 3,000 (mJ / cm 2 ), and more preferably 200 to 2,000 (mJ / cm 2 ), and more preferably 300 to 1,500 (mJ / cm 2 ) where UV illuminance is the radiation intensity received per unit area, and varies with lamp output, emission spectral efficiency, diameter of the light-emitting bulb, design of the reflector, and the distance between the irradiated object and the light source. However, illuminance does not vary with transport speed. Additionally, the integrated UV light quantity is the radiation energy received per unit area, and is the total amount of photons that reach the surface. The integrated light quantity is inversely proportional to the radiation speed passing under the light source, and proportional to the number of irradiations and the number of lamps.
[0112] The method for peeling off the supporting substrate in step 4 is not particularly limited as long as the supporting substrate and the resin film can be peeled off uniformly. Generally, however, a method in which the resin film side is fixed via an adhesive layer or the like, and then the supporting substrate side is peeled off is preferred.
[0113] [Resin precursor] The resin precursor is not particularly limited as long as it is a compound having a site that can be crosslinked, but A resin precursor containing the structure of Chemical Formula 4 is preferred, and a resin precursor containing the structure of Chemical Formula 5 is more preferred.
[0114] [ka]
[0115] [ka]
[0116] As described above, the structures of Chemical Formulas 4 and 5 have a (meth)acrylic group at the end, which is represented by X in the diagram, and this (meth)acrylic group (X) at the end is a site that can be crosslinked. Furthermore, the (meth)acrylic group (X) is adjacent to a polyisocyanate residue represented by Y in the figure. 5 The segment is represented by the other end of the polyisocyanate residue represented by Y and the chemical formula 5 This means that the polyol residues (Z) represented by Z in the formula (1) are adjacent to each other.
[0117] The polyisocyanate residue (Y) of Chemical Formulas 4 and 5 is preferably a residue of a polyisocyanate such as TDI (tolylene diisocyanate), MDI (4,4'-diphenylmethane diisocyanate), NDI (1,5-naphthalene diisocyanate), TODI (tolidine diisocyanate), XDI (xylylene diisocyanate), PPDI (paraphenylene diisocyanate), TMXDI (tetramethylxylylene diisocyanate), HMDI (hexamethylene diisocyanate), IPDI (isophorone diisocyanate), H6XDI (hydrogenated xylylene diisocyanate), or H12MDI (dicyclohexylmethane diisocyanate).
[0118] The polyol residue of Chemical Formula 5 is preferably a polyester polyol, a polyether polyol, or a polycarbonate polyol.
[0119] [Coloring agent] The colorant is not particularly limited as long as it is used to color the resin film, reduce the total light transmittance, and impart hiding properties, and can form a resin film that exhibits the characteristics of the present invention; however, it is preferable that the colorant is suitable for the manufacturing method of the laminate described above.
[0120] As shown below, colorants can be divided into pigments and dyes, with pigments being preferred from the standpoint of hiding power efficiency and weather resistance of the resin film.
[0121] Pigments include black, white, red, green, blue, yellow, purple, cyan, magenta, etc., and these may be used alone or in combination of two or more. In order to prevent deterioration of quality due to the generation of colorant aggregates, it is preferable to reduce the content of the colorant as much as possible, and it is preferable to use a black pigment alone.
[0122] Examples of black pigments include carbon compounds such as carbon black, graphite, fullerene, carbon fiber, and carbon nanotubes (CNT), and inorganic oxides such as titanium black, aniline black, perylene black, manganese oxide, ferrous oxide, cupric oxide, cobalt oxide, bismuth oxide, chromium oxide, and magnetite. Of these, carbon black is particularly preferred because of its excellent hiding power.
[0123] Examples of the white pigment include inorganic oxides such as calcium carbonate, barium sulfate, and titanium dioxide.
[0124] Examples of red and magenta pigments include, for example, CI Pigment Red 7, 9, 14, 41, 48:1, 48:2, 48:3, 48:4, 57:1, 81, 81:1, 81:2, 81:3, 81:4, 122, 123, 146, 155, 166, 168, 176, 177, 178, 180, 184, 185, 187, 200, 202, 208, 209, 210, 217, 220, 224, 242, 246, 254, 255, 264, 270, 272, and 279, in terms of color index names.
[0125] Examples of green pigments include CI Pigment Green 1, 2, 4, 7, 8, 10, 13, 14, 15, 17, 18, 19, 26, 36, 45, 48, 50, 51, 54, 55 and 58, etc., in terms of color index names.
[0126] Examples of blue and cyan pigments include, by color index name, CI Pigment Blue 1, 1:2, 9, 14, 15, 15:1, 15:2, 15:3, 15:4, 15:6, 16, 17, 19, 25, 27, 28, 29, 33, 35, 36, 56, 56:1, 60, 61, 61:1, 62, 63, 66, 67, 68, 71, 72, 73, 74, 75, 76, 78, and 79.
[0127] Yellow pigments are, for example, CI Pigment Yellow 1, 2, 3, 4, 5, 6, 10, 12, 13, 14, 15, 16, 17, 18, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 42, 43, 53, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 83, 93, 94, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 115, 1 16, 117, 118, 119, 120, 123, 126, 127, 128, 129, 138, 139, 147, 150, 151, 152, 153, 154, 155, 156, 161, 162, 164, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 179, 180, 181, 182, 184, 185, 187, 188, 193, 194, 198, 199, 213 and 214.
[0128] Examples of the dye include black dyes such as azo-based metal complex salt dyes, and organic compounds such as anthraquinone-based compounds.
[0129] [Paint composition] The "coating composition" used in the method for producing a laminate of the present invention is not particularly limited as long as it can be applied uniformly in-plane on a supporting substrate and can form a resin film exhibiting the characteristics of the present invention, but it is preferable that the coating composition is suitable for the method for producing the laminate described above. Specifically, it is preferable to prepare a coating composition by adding the above-mentioned resin precursor to a solvent, colorant, and other components described below. In addition, when using a colorant that has poor dispersibility in a coating composition such as a pigment, it is preferable to disperse the pigment in two stages. Specifically, it is more preferable to prepare a "pigment dispersion" once by adding and dispersing the pigment to a resin precursor and a solvent so that the pigment is at a higher concentration than the pigment addition amount used in this application, and then diluting this with a resin precursor and a solvent to prepare a coating composition.
[0130] [solvent] The coating composition used in the method for producing the laminate of the present invention may contain a solvent, and it is preferable to contain a solvent in order to form a coating layer uniformly in the plane. The number of types of solvents is preferably 1 to 20, more preferably 1 to 10, even more preferably 1 to 6, and particularly preferably 1 to 4. Here, the term "solvent" refers to a substance that is liquid at room temperature and normal pressure and can be evaporated almost entirely in the drying process described above.
[0131] Here, the type of solvent is determined by the molecular structure that constitutes the solvent. In other words, solvents that have the same elemental composition and the same type and number of functional groups but different bond relationships (structural isomers), and solvents that are not structural isomers but do not overlap exactly in any conformation in three-dimensional space (stereoisomers) are treated as different types of solvents. For example, 2-propanol and n-propanol are treated as different solvents.
[0132] [Other components in the coating composition] The coating composition used in the method for producing the laminate of the present invention preferably contains an antioxidant, a polymerization initiator, a curing agent, and a catalyst. The polymerization initiator and catalyst are used to promote crosslinking of the resin film. The polymerization initiator is preferably one that can initiate or promote polymerization, condensation, or crosslinking reaction of the components contained in the coating composition by anionic, cationic, or radical polymerization reaction, etc.
[0133] Antioxidants are broadly classified into radical chain initiation inhibitors, radical scavengers, and peroxide decomposers based on their mechanism of action, and although any of these can provide the effect of the present invention in terms of inhibiting deterioration under high temperature conditions, radical scavengers or peroxide decomposers are more preferred, and hindered phenol-based or semi-hindered phenol-based radical scavengers, or phosphite-based or thioether-based peroxide decomposers are more preferred. When carbon black is used to impart hiding power, it is more preferred to include a hindered phenol-based radical scavenger in order to improve the dispersibility of the carbon black.
[0134] Various polymerization initiators, curing agents, and catalysts can be used. The polymerization initiators, curing agents, and catalysts may be used alone, or multiple polymerization initiators, curing agents, and catalysts may be used simultaneously. Furthermore, an acid catalyst or a thermal polymerization initiator may be used in combination. Examples of acid catalysts include hydrochloric acid aqueous solution, formic acid, and acetic acid. Examples of thermal polymerization initiators include peroxides and azo compounds. Examples of photopolymerization initiators include alkylphenone compounds, sulfur-containing compounds, acylphosphine oxide compounds, and amine compounds. Examples of crosslinking catalysts that promote the reaction of forming urethane bonds include dibutyltin dilaurate and dibutyltin diethylhexoate.
[0135] As the photopolymerization initiator, it is preferable to use an alkylphenone compound and an acylphosphine oxide compound in combination from the viewpoint of curability. Specific examples of the alkylphenone compound include 1-hydroxy-cyclohexyl-phenyl-ketone, 2,2-dimethoxy-1,2-diphenylethane-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-phenyl)-1-butane, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-(4-phenyl)-1-butane, 2-benzyl-2-dimethylamino-1-(4- morpholinophenyl)-1-butane, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butane, 1-cyclohexyl-phenyl ketone, 2-methyl-1-phenylpropan-1-one, 1-[4-(2-ethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, bis(2-phenyl-2-oxoacetate)oxybisethylene, and materials that have been made into high molecular weights. Specific examples of acylphosphine oxide compounds include 2,4,6-trimethylbenzoyl-diphenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, and materials that have been made into high molecular weights. These may be used alone or in combination of two or more.
[0136] In addition, a leveling agent, a lubricant, an antistatic agent, etc. may be added to the coating composition used to form the resin film as long as the effects of the present invention are not impaired. As a result, the resin film can contain a leveling agent, a lubricant, an antistatic agent, etc.
[0137] Examples of the leveling agent include acrylic copolymers, silicone-based, and fluorine-based leveling agents. Examples of the antistatic agent include metal salts such as lithium salts, sodium salts, potassium salts, rubidium salts, cesium salts, magnesium salts, and calcium salts.
[0138] [Application example] The resin film of the present invention has advantages such as excellent optical properties, flexibility, stretchability, transportability, and appearance quality, and can be suitably used in applications where particularly high flexibility and stretchability are required.
[0139] For example, the resin film can be suitably used for the surface, internal, structural, and manufacturing process materials of plastic molded products such as glasses / sunglasses, cosmetic cases, and food containers, aquariums, showcases for exhibitions, smartphone housings, touch panels, color filters, flat panel displays, flexible displays, flexible devices, wearable devices, sensors, circuit materials, electrical and electronic applications, home appliances such as keyboards, television and air conditioner remote controls, mirrors, window glass, buildings, dashboards, car navigation touch panels, vehicle parts such as room mirrors and windows, and various printed matter, medical films, sanitary material films, medical films, agricultural films, building material films, etc. The quality of these materials can be improved by using the resin film of the present invention. EXAMPLES
[0140] Next, the present invention will be described based on examples, but the present invention is not necessarily limited to these. In the following, Examples 6 to 8 will be read as Reference Examples 6 to 8. "Synthesis of resin precursors" In the synthesis of the resin precursor, the raw materials used are as follows:
[0141] "Diisocyanate" IPDI: Isophorone diisocyanate ·MDI: 4,4'-diphenylmethane diisocyanate "Polyol" PBAA-1: Polybutylene adipate, Tosoh Corporation, Nipponran 3027 (weight average molecular weight 2500) PEAA: Polyethylene glycol adipate, Tosoh Corporation, Nipporan 4040 (Weight average molecular weight 2000) EX861: Polyethylene glycol diglycidyl ether, Nagase ChemteX Corporation "Hydroxy acrylate" ·HEA: Hydroxyethyl acrylate 4HBA: 4-Hydroxybutyl acrylate GMA: Glycidyl methacrylate "Bisphenol A epoxy compound" YD8125: Manufactured by Nippon Steel Chemical and Materials Co., Ltd. "Succinic anhydride" "Rikacid" (registered trademark) SA: Manufactured by New Japan Chemical Co., Ltd. [Resin precursor A] In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, IPDI as a diisocyanate, PBAA-1 as a polyol, and toluene were placed. At this time, the molar ratio of diisocyanate to polyol was set to 0.43:0.29, and the solid content concentration was set to 60% by mass. The reaction was carried out at 90°C, and when the remaining isocyanate groups in the unreacted state were taken as 100% by mass, the temperature was lowered to 70°C when the remaining isocyanate groups became 1.4% by mass due to the reaction, and hydroxyacrylate (HEA) was added. At this time, the molar ratio of diisocyanate to polyol to hydroxyacrylate in the unreacted state was set to 0.43:0.29:0.29. When the amount of remaining isocyanate groups before reaction was taken as 100% by mass, the reaction was terminated by stopping heating when the amount of remaining isocyanate groups reached 0.3% by mass. Toluene was then added to adjust the solids concentration to 60% by mass, thereby obtaining a toluene solution of resin precursor A. [Resin precursor B] In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, IPDI as a diisocyanate, PBAA-1 as a polyol, and toluene were placed. At this time, the molar ratio of diisocyanate to polyol was set to 0.48:0.32, and the solid content concentration was set to 60% by mass. The reaction was carried out at 90°C, and when the remaining isocyanate groups in the unreacted state were taken as 100% by mass, the temperature was lowered to 70°C when the remaining isocyanate groups became 1.4% by mass due to the reaction, and hydroxyacrylate (HEA) was added. At this time, the molar ratio of diisocyanate to polyol to hydroxyacrylate in the unreacted state was set to 0.48:0.32:0.20. When the amount of remaining isocyanate groups before reaction was taken as 100% by mass, the reaction was terminated by stopping heating when the amount of remaining isocyanate groups reached 0.3% by mass. Toluene was then added to adjust the solids concentration to 60% by mass, thereby obtaining a toluene solution of resin precursor B. [Resin precursor C] In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, MDI as a diisocyanate, PEAA as a polyol, and toluene were placed. At this time, the molar ratio of diisocyanate to polyol was set to 0.43:0.29, and the solid content concentration was set to 60 mass%. The reaction was performed at 90°C, and when the remaining isocyanate group became 1.4 mass% due to the reaction, the temperature was lowered to 70°C, and hydroxyacrylate (HEA) was added. At this time, the molar ratio of diisocyanate to polyol to hydroxyacrylate at the time of unreacting was set to 0.43:0.29:0.29. When the amount of remaining isocyanate groups before reaction was taken as 100% by mass, the reaction was terminated by stopping heating when the amount of remaining isocyanate groups reached 0.3% by mass. Toluene was then added to adjust the solids concentration to 60% by mass, thereby obtaining a toluene solution of resin precursor C. [Resin precursor D] As resin precursor D, NK Oligo (weight average molecular weight 4000) manufactured by Shin-Nakamura Chemical Co., Ltd., which is a bisphenol A type epoxy acrylate, was used. [Resin precursor E] In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a nitrogen gas inlet, 64.8 parts of bisphenol A, 57.1 parts of bisphenol A type epoxy compound (YD8125), 128.1 parts of polyethylene glycol diglycidyl ether (EX861), 1.25 parts of triphenylphosphine as a catalyst, 1.25 parts of N,N-dimethylbenzylamine, and toluene as a solvent were charged, so that the solid content concentration was 60% by mass. The mixture was heated to 110°C while stirring under a nitrogen stream and reacted for 8 hours to obtain a hydroxyl group-containing resin. Next, 54.6 parts of succinic anhydride ("Rikacid" (registered trademark) SA) was added as an acid anhydride, and the mixture was reacted for 4 hours at 110°C. After confirming that the absorption of the acid anhydride group had disappeared by FT-IR measurement, the mixture was cooled to room temperature. Next, the introduction of nitrogen from the nitrogen inlet tube was stopped and replaced with dry air, and 26.0 parts of glycidyl methacrylate (GMA) was added to the flask with stirring, and the mixture was allowed to react for 8 hours at 80° C. After completion of the reaction, methyl ethyl ketone was added to adjust the solid content to 50% by mass, thereby obtaining a methyl ethyl ketone solution of resin precursor E. "Preparation of colorant dispersion" The colorants and dispersants used are as follows: "Coloring agent" "Niteron" (registered trademark) #10MAF: Carbon black, manufactured by Nippon Steel Carbon Corporation, average particle size 40 nm ·“Lumogen” (registered trademark) Black FK4280: Perylene black manufactured by BASF, average 30 nm ·Kayaset Black AN: Anthraquinone black dye, manufactured by Nippon Kayaku Co., Ltd. · Cyanine Blue 5191: Phthalocyanine Blue manufactured by Dainichi Seika Chemicals Co., Ltd. "Dispersant" ·BYK111: Dispersant manufactured by BYK-Chemie Co., Ltd. [Colorant dispersion A] A mixing vessel was charged with 1 part by mass of carbon black, 0.2 parts by mass of BYK111, and 0.5 parts by mass of Cyan Blue, and the solids concentration was adjusted to 5% by mass with methyl ethyl ketone to obtain colorant dispersion A. [Colorant dispersion B] A mixing vessel was charged with 1 part by mass of perylene black, 0.2 parts by mass of BYK111, and 0.5 parts by mass of Cyan Blue, and the solids concentration was adjusted to 5% by mass with methyl ethyl ketone to obtain colorant dispersion B. [Colorant dispersion C] In a mixing vessel, an anthraquinone-based black dye was adjusted with methyl ethyl ketone so that the solid content concentration was 5 mass %, and a colorant dispersion C was obtained. [Colorant dispersion D] Colorant dispersion A was added to a mixing vessel, and then resin precursor A was added thereto so that the amount was 16 parts by mass per part by mass of carbon black. The mixture was then diluted with methyl ethyl ketone so that the overall solids concentration was 55% by mass, thereby obtaining colorant dispersion D. [Colorant dispersion E] Colorant dispersion A was added to a mixing vessel, and then resin precursor B was added thereto so that the amount was 16 parts by mass per 1 part by mass of carbon black. The mixture was then diluted with methyl ethyl ketone so that the total solids concentration was 55% by mass, thereby obtaining colorant dispersion E. [Paint composition formulation] The resin precursor, colorant dispersion, and additive types and solid content ratios were as shown in Table 1, and these materials were diluted with methyl ethyl ketone to obtain a resin film-forming coating composition with a solid content concentration of 40 mass %. In this case, the additives refer to a group consisting of photopolymerization initiators, leveling agents, antioxidants, and heat curing agents, and the raw materials used are as follows. "Additives" Photopolymerization initiator A: “IRGACURE” (registered trademark) 184 (manufactured by BASF Japan Ltd.) Photoinitiator B: “Omnirad” (registered trademark) TPO (manufactured by IGM Resins) Leveling agent A: “Megafac” (registered trademark) F-556 (manufactured by DIC Corporation) Antioxidant A: “Irganox” (registered trademark) 1010 (manufactured by BASF Japan Ltd.) Heat curing agent A: “Desmodur” (registered trademark) BL-4265SN (isocyanate equivalent weight = 337g / eq) manufactured by Sumika Covestro Urethane Co., Ltd. Heat curing agent B: “Duranate” (registered trademark) E402-B80B (isocyanate equivalent = 560g / eq) manufactured by Asahi Kasei Chemicals Corporation
[0142] [Table 1]
[0143] [Release layer coating composition] The following materials were mixed and diluted with a mixed solvent of methyl ethyl ketone / isopropyl alcohol (mixture ratio by mass: 50 / 50) to obtain a coating composition for a release layer having a solids concentration of 5% by mass. Side-chain carbinol modified reactive silicone oil (X-22-4015 Shin-Etsu Chemical Co., Ltd. Solid content: 100% by mass): 5 parts by mass ·Both-end polyether modified reactive silicone oil (X-22-4952 Shin-Etsu Chemical Co., Ltd. Solid content: 100% by mass): 5 parts by mass Acrylic modified alkyd resin solution (Hariftar KV-905, Harima Chemicals Co., Ltd., solid content concentration 53% by mass): 100 parts by mass Isobutyl alcohol modified melamine resin solution “Melan” (registered trademark) 2650L Hitachi Chemical Co., Ltd. Solid content concentration 60% by mass: 20 parts by mass · Paratoluenesulfonic acid: 5 parts by weight. [Method of manufacturing laminate and resin film] [Formation of Support Substrate with Release Layer] Using a coating device with a small diameter gravure coater, the release layer coating composition was applied to a 50 μm thick polyester film (manufactured by Toray Industries, Inc., under the trade name "Lumilar" (registered trademark) R75X) by adjusting the line count of the gravure roll, the peripheral speed of the gravure roll, and the solids concentration of the release layer coating composition so that the release layer thickness would be approximately 200 nm. The film was then dried and crosslinked by holding it at a hot air temperature of 140°C for 30 seconds, thereby obtaining a support substrate with a release layer. [Laminate formation method A] (Process 1) The support substrate with the release layer described above was used as the support substrate, and the coating composition described above was applied onto the release layer of the support substrate using a continuous coating device with a slot die coater, with the discharge flow rate adjusted so that the thickness of the resin film after crosslinking would be the specified film thickness, to form a coating layer.
[0144] (Process 2) The coating layer formed in step 1 was dried under the following conditions to remove the solvent.
[0145] Air blowing temperature: Temperature: 50℃, Wind speed: Coating side: 5m / sec, non-coating side: 5m / sec Air direction: Coating side: Parallel to the surface of the substrate, Non-coating side: Perpendicular to the surface of the substrate Dwell time: 2 minutes (Step 3) In step 2, the coating layer (uncrosslinked resin film) obtained by removing the solvent was crosslinked by irradiating it with active energy rays under the conditions described below to obtain a laminate consisting of a supporting substrate, a release layer and a resin film.
[0146] Irradiation light source: High pressure mercury lamp Irradiation power: 400W / cm 2 Accumulated light output: 120mJ / cm 2 Oxygen concentration: 0.1% by volume.
[0147] [Laminate formation method B] A laminate was obtained by changing the air temperature in step 2 to 80° C. and maintaining the other conditions in the same manner as in laminate formation method A.
[0148] By the above-mentioned method, the laminates and resin films were prepared in Examples 1 to 8 and Comparative Examples 1 to 4. The coating composition for forming a resin film, the method for forming the laminate, and the thickness of each resin film corresponding to each Example and Comparative Example are shown in Table 2.
[0149] [Table 2]
[0150] [Evaluation of resin films and laminates] The laminates and resin films were subjected to the following performance evaluations, and the results are shown in Table 2. Unless otherwise specified, measurements were taken three times for one sample in each Example and Comparative Example at different locations, and the average value was used.
[0151] [Measurement of storage modulus and loss tangent of resin film] The laminate was cut into a rectangle having a width of 10 mm, and the supporting substrate was peeled off to prepare a test piece.
[0152] Based on the tensile vibration-non-resonance method of JIS K7244-4 (1999) (this is called the dynamic viscoelasticity method), the storage modulus and loss tangent of the resin film were determined using a dynamic viscoelasticity measuring device "DMS6100" manufactured by Seiko Instruments Inc. Measurement mode: Tensile Chuck distance: 20mm Test piece width: 10mm Frequency: 1Hz Distortion amplitude: 10μm Minimum tension: 20mN Initial force amplitude: 40mN Measurement temperature: -100℃ to 200℃ Heating rate: 5℃ / min [Measurement of total light transmittance of resin film] The laminate was cut into a 50 mm square, and the supporting substrate was peeled off to prepare a test piece.
[0153] Based on JIS K7375 (2008), the total light transmittance of the resin film was determined using a haze meter NDH-5000 manufactured by Nippon Denshoku Co., Ltd. [Particle size analysis of colorants contained in resin film] The particle size analysis of the colorant present in the resin film was carried out by cross-sectional SEM observation of the film using a SEM JSM-6700F manufactured by JEOL Ltd. The procedure for preparing a test piece for cross-sectional SEM observation was as follows.
[0154] 1. The resin film side of the laminate was embedded in UV-curable resin. The supporting substrate was then peeled off, and the same procedure was carried out.
[0155] 2. Using a rotary microtome RMS manufactured by Nippon Microtome Co., Ltd., the resin film together with the embedded resin was cut at 10 μm intervals in the TD direction of the sample.
[0156] 3. Using an Auto Fine Coater JFC-1600 manufactured by JEOL Ltd., platinum was deposited to a thickness of approximately 10 μm on the cut cross section of the sample (conditions: 30 mA x 20 seconds x 2 times) to prepare a test piece.
[0157] The cross-sectional SEM observation was performed under the following conditions. Measurement mode: LEI mode Magnification: 5000x Acceleration voltage: 3 kV WD (sample distance): 8.0 mm Particle size analysis of the colorant contained in the resin film was performed on cross-sectional SEM images using the image analysis software ImageJ (developed by the National Institutes of Health, USA) according to the following procedure. 1. The images were trimmed and combined so that the entire thickness direction of the film cross section was included without overlapping. In addition, the images were trimmed so that parts unrelated to the film cross section were not displayed. 2. The cross-sectional SEM images were converted to 8-bit. 3. The cross-sectional SEM image was processed by Smooth and Sharpen twice, then Find Edge and Smooth once each to enhance the contours of the image. 4. Adjust the Brightness / Contrast so that only the colorant particles are white. 5.The whitened areas were selected using threshold and binarized. 6. Analyze Particles to analyze the particle size of the colorant. At this time, select Ellipses in the show tab to perform elliptical approximation. 7. The above image analysis was performed on three cross-sectional SEM images of each sample, and the occupied area ratio and the long and short diameters of each particle were calculated. The particle diameter of each colorant particle was defined as (long diameter + short diameter) / 2. 8. Create a frequency distribution of the particle size of the analyzed colorant, and define the particle size with the frequency closest to 50% as D 50 The particle size with the frequency closest to 95% is D 95 It was defined as follows. 9. Using the following formula, D in the region of 30% to 70% of the resin film thickness 50 and D 95 From the value of F A D in the range of 0% to 30% and 70% to 100% of the resin film thickness 50 and D 95 From the value of F B were calculated, respectively.
[0158] F A =D 95 (30%~70% area) / D 50 (30%~70% area) F B =D 95 (0%~30%, 70%~100% area) / D 50 (0%~30%, 70%~100% area) [Measuring resin film thickness] The arithmetic mean value of the thicknesses obtained from the cross-sectional SEM images was regarded as the thickness of the resin film.
[0159] [Peel strength between support substrate and resin film] In the laminate, the resin film and the supporting substrate were peeled off slightly from the edge to form a gripping area for measurement with a tensile tester (Orientec Tensilon UCT-100). Next, the resistance value (N) was measured when peeled off at 180 degrees at a speed of 1200 (mm / min) using the tensile tester in a 23°C, 65% RH environment. The resistance value (N) was divided by the width (mm) of the supporting substrate and the resin film, then multiplied by 50 to convert it into a peel force (N / 50mm) equivalent to a width of 50mm for each.
[0160] [Evaluation of resin film flexibility] The laminate was cut into a rectangle of 10 mm width x 150 mm length, and the resin film was peeled off from the support substrate to prepare a test piece. The direction of the 150 mm length was aligned with the longitudinal direction of the resin film. Using a tensile tester (Orientec Tensilon UCT-100), the initial tensile chuck distance was set to 50 mm, the tensile speed was set to 300 mm / min, and the measurement temperature was set to 23°C.
[0161] Read the load b (N) applied to the sample when the chuck distance is a (mm), and use the following formula to calculate the strain x (%) and stress y (N / mm 2 ) was calculated, where k (mm) is the sample thickness before the test. Strain amount: x = ((a-50) / 50) x 100 Stress: y=b / (k×10).
[0162] Of the data obtained above, the stress at a strain of 5% was defined as the 5% strain stress, and a value of 5 MPa or less was deemed acceptable.
[0163] [Evaluation of Resin Film Restoration] The resin film was cut into a rectangle measuring 10 mm wide x 150 mm long to prepare a test piece. The direction of the 150 mm long was aligned with the longitudinal direction of the resin film. Using a tensile tester (Orientec Tensilon UCT-100), the test was performed at a measurement temperature of 23°C under two conditions with different deformation speeds to determine the superiority or inferiority of the restoring ability.
[0164] Condition A: Initial chuck distance 50 mm, tensile speed 50 mm / min. After stretching the sample to 100% strain, release the tensile load on the sample and measure the distance marked as the initial test length before the measurement. The elastic recovery rate z1 (%) and shear rate s1 (s -1 ) was calculated.
[0165] Elastic recovery rate z1 = (1-(L-50) / 100) x 100 (%).
[0166] Shear rate s1 = (50 / 60) / 10 = 0.08 (s -1) Condition B: Initial chuck distance 50 mm, tensile speed 300 mm / min. After the sample was stretched to a strain of 100%, the tensile load on the sample was released, and the distance marked as the initial test length before the measurement was measured and recorded as L mm. The elastic recovery rate z1% was calculated using the following formula.
[0167] Elastic recovery rate z2 = (1-(L-50) / 100) x 100 (%).
[0168] Shear rate s1 = (50 / 60) / 10 = 0.08 (s -1 ) In the above evaluation, condition A was considered to be 90% or more and condition B was 70% or more, respectively, to be a pass.
[0169] [Evaluation of the Concealment Ability of Resin Film] The hiding power of the film was evaluated by the following two methods, and a film that passed at least condition A was rated as passing.
[0170] Condition A: Draw five 40mm lines at 5mm intervals on general-purpose white cardboard (HSK Ivory, manufactured by Hisada Shoeido Co., Ltd.) using a black magic marker (Tombow Pencil Co., Ltd.'s Oil-based Twin Marker Extra Fine Mono Twin E Black). Place the aforementioned white cardboard and resin film, in that order, on a light box equipped with a high color rendering fluorescent lamp (40W). Expose to light and visually observe from above. If the spacing between the black marker lines cannot be recognized, the test is deemed to have passed.
[0171] Condition B: The laminate was cut into 50 mm squares, the support substrate was peeled off, and test pieces were prepared. The total light transmittance was measured by the above-mentioned method, and then the test pieces were stored for one week in a humid and hot environment (85°C, 85% RH) using a constant temperature chamber LHL-113 manufactured by Espec Corp. Thereafter, the test pieces were left to stand for one hour or more in an atmosphere of 23°C and 65% RH, after which the total light transmittance was measured again, and the rate of change was calculated. [Evaluation of the appearance quality of resin film] The resin film was visually observed, and the resin film was 2 Based on the number of defects found within the sample, a score was assigned as follows and the sample was evaluated.
[0172] 5 points: 3 or less defects smaller than 10 mm 4 points: 3 to 5 defects less than 10 mm 3 points: 5 to 7 defects less than 10 mm in size 2 points: 7 to 10 defects of 10 mm or less 1 point: 10 or more defects less than 10 mm, or 1 or more defects 10 mm or larger.
[0173] Table 3 shows the structure of Chemical Formula 1 of the resin film and whether or not it contains a urethane bond, Table 4 shows the evaluation results of conditions 1 to 6 mentioned above, and Table 5 shows the evaluation results of the flexibility, recovery, hiding power, and appearance quality of the resin film.
[0174] [Table 3]
[0175] [Table 4]
[0176] [Table 5]
[0177] In Table 3, "includes" in the column for the structure of Chemical Formula 1 means that each Example contains the structure of Chemical Formula 1, and "does not include" means that each Example does not contain the structure of Chemical Formula 1. The same applies to the urethane bond. [Explanation of symbols]
[0178] 1, 4, 8, 12, 17, 21, 26, 32: Laminate 2, 5, 9, 13, 18, 22, 27, 33: Resin film 6, 10, 14, 15, 23, 28, 30, 34: Release layer 3, 7, 11, 16, 19, 24, 29, 35: Supporting base material 20, 25, 31, 37: Protective material 36: Adhesive layer [Industrial Applicability]
[0179] The resin film of the present invention has advantages such as excellent optical properties, flexibility, stretchability, transportability, and appearance quality, and can be suitably used in applications where particularly high flexibility and stretchability are required.
[0180] To name a few examples, it can be suitably used for the surface materials, internal materials, constituent materials, and manufacturing process materials of plastic molded products such as glasses / sunglasses, cosmetic cases, and food containers, aquariums, showcases for exhibitions, smartphone housings, touch panels, color filters, flat panel displays, flexible displays, flexible devices, wearable devices, sensors, circuit materials, electrical and electronic applications, home appliances such as keyboards, remote controls for televisions and air conditioners, mirrors, window glass, buildings, dashboards, car navigation touch panels, vehicle parts such as rearview mirrors and windows, and various printed matter, medical films, films for sanitary materials, medical films, agricultural films, and building materials.
Claims
1. A resin film comprising a crosslinked product of a resin precursor containing a structure of chemical formula 5, and satisfying all of the following conditions 1 to 5: [Case 1] In addition, R in Chemical Formula 5 7 refers to a hydrogen or a methyl group. In addition, R in Chemical Formula 5 9 refers to a substituted or unsubstituted alkylene group. The polyol residue (Z) in Chemical Formula 5 is any one of a polyester polyol, a polyether polyol, and a polycarbonate polyol. Condition 1: The resin film contains a pigment. Condition 2: The total light transmittance of the resin film measured by the method specified in JIS K7375 (2008) is 2% or more and 20% or less. Condition 3: The storage modulus of the resin film at a temperature of 25° C. and a frequency of 1 Hz is 0.5 MPa or more and 50 MPa or less. Condition 4: The loss tangent of the resin film at 25° C. is 0.5 or less. Condition 5: The occupied area ratio of the pigment in the cross section of the resin film is 0.1% or more and 2.0% or less.
2. The resin film according to claim 1 , which satisfies the following condition 6: Condition 6: The 95% particle diameter (D 95 ) and 50% particle size (D 50 ) is the ratio of F A The ratio of the average value of D95 and D50 of the pigment in the area from the surface to 0% to 30% and the area from 70% to 100% in the thickness direction is F. B When this is set, formula 1 and formula 2 are satisfied. Formula 1: F A <2.4 Formula 2: |F A -F B | < 0.4
3. The resin film according to claim 1 or 2, wherein the pigment is a black pigment.
4. The resin film according to claim 3 , which satisfies condition 7. Condition 7: The absorption coefficient of the resin film (ε A ) satisfies Equation 3. Equation 3: ε A (1 / μm)=100×(Log 10 100 / T) / (A×d)>2.0 where A is the occupied area ratio (%) of the black pigment, d is the thickness (μm) of the resin film, and T is the total light transmittance (%) of the resin film.
5. The resin film according to any one of claims 1 to 4, which satisfies the following conditions 3' and 4'. Condition 3': The storage modulus of the resin film at a temperature of 25° C. and a frequency of 1 Hz is 3.0 MPa or more and 10 MPa or less. Condition 4': The loss tangent of the resin film at 25°C is 0.2 or less.
6. 6. A laminate having a supporting substrate on at least one surface of the resin film according to claim 1, wherein the peel strength between the supporting substrate and the resin film is 1 N / 50 mm or less.
7. A display member comprising the resin film according to any one of claims 1 to 5.
8. A healthcare sensor comprising the resin film according to any one of claims 1 to 5.
Citation Information
Patent Citations
Pulse train generating circuit
JP1988065712A
Black photosensitive composition, solder resist and photosensitive dry film
JP2012141605A
Uv-curing resin composition
JP2013194156A
Dry resist film, electromagnetic wave shield sheet-attached printed wiring board, and method for manufacturing the same
JP2018152606A
Black photosensitive resin composition
JP2018163336A