Thermoplastic elastomer composition, molded body, and instrument panel skin

A thermoplastic elastomer composition with specific components improves flexibility and breakability, addressing the limitations of existing materials for instrument panels, particularly in low-temperature environments, ensuring effective airbag deployment.

JP7567194B2Active Publication Date: 2024-10-16MITSUBISHI CHEM CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020060664
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-03-30
Publication Date
2024-10-16
Estimated Expiration
2040-03-30

AI Technical Summary

Technical Problem

Existing thermoplastic elastomer compositions used in automobile instrument panels lack sufficient flexibility and easy breakability, especially in lower temperature environments, which is crucial for effective airbag deployment.

Method used

A thermoplastic elastomer composition containing ethylene/propylene/nonconjugated diene copolymer rubber, olefin resin, hydrogenated copolymer of a vinyl aromatic compound and conjugated diene, and a crosslinking agent, with specific proportions and softeners, to enhance flexibility and breakability across a wide temperature range.

Benefits of technology

The composition achieves both excellent flexibility and easy breakability, enabling effective airbag deployment in a wide temperature range, enhancing safety and application suitability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567194000001
    Figure 0007567194000001
Patent Text Reader

Abstract

To provide a thermoplastic elastomer composition which achieves both easy breaking property and excellent flexibility in a wide temperature region, and enables easy development of a skin during air bag development when being used as a skin for an instrument panel.SOLUTION: There are provided a thermoplastic elastomer composition which contains the following components (a) to (d), contains 1-20 mass% of the component (c) with respect to 100 mass% of the total of the components (a) to (d), and is crosslinked with the following component (e); a molding obtained by molding the thermoplastic resin composition; and a skin for an instrument panel which is composed of the thermoplastic elastomer composition. Component (a): ethylene-propylene-non-conjugated diene copolymer rubber. Component (b): olefinic resin. Component (c): hydrogenated product of a copolymer of a vinyl aromatic compound and conjugated diene having a glass transition temperature of 0°C or higher. Component (d): softening agent for hydrocarbon-based rubber. Component (e): crosslinking agent.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermoplastic elastomer composition. More specifically, the present invention relates to a thermoplastic elastomer composition having excellent flexibility and breakability, a molded article obtained by molding the thermoplastic elastomer composition, and a surface layer for an instrument panel made of the thermoplastic elastomer composition. [Background technology]

[0002] Conventionally, automobile interior sheets used as the surface of instrument panels have been made of laminates in which polyvinyl chloride with a leather pattern embossed on the surface, a foam layer, and, if necessary, a resin substrate layer are laminated in sequence. However, in order to meet the needs for weight reduction, recyclability, and ease of incineration of automobiles, as well as environmental issues, heat resistance, cold resistance, heat aging resistance, weather resistance, low odor, flexibility, and a luxurious feel, polyolefin thermoplastic elastomers (TPOs) have been put to practical use in recent years.

[0003] Examples of TPO that can be used for such automotive interior skins include ethylene-α-olefin-non-conjugated diene copolymer rubber, polypropylene resin, and high-pressure processed TPO with a density of 0.910 to 0.940 g / cm. 3 A thermoplastic elastomer composition is known which is obtained by subjecting polyethylene to dynamic heat treatment in the presence of an organic peroxide (see Patent Document 1). Patent Document 1 describes a thermoplastic elastomer composition which is obtained by subjecting an ethylene-α-olefin-non-conjugated diene copolymer rubber and a polyethylene terephthalate (PE) having a density of 0.910 to 0.940 g / cm produced by a high pressure method. 3 It is described that by using this in combination with polyethylene, it is possible to improve the ease of breaking over a wide temperature range from low temperature (about -20°C) to high temperature (about 85°C). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2016-11396 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, there has been a demand for airbag deployment performance in lower temperature environments. In order to achieve good airbag deployment performance in such low temperature environments, there is a demand for a materials approach to develop a thermoplastic elastomer that has excellent breakability even in lower temperature ranges while maintaining the inherent flexibility of the thermoplastic elastomer composition. The thermoplastic elastomer composition described in Patent Document 1 uses a relatively hard polyethylene to obtain easy breakability over a wide temperature range, and there is room for improvement in applications requiring greater flexibility.

[0006] An object of the present invention is to solve the above-mentioned problems associated with conventional products, and to provide a thermoplastic elastomer composition which combines easy breakability over a wide temperature range with excellent flexibility and which, when used as an instrument panel skin, enables the skin to easily deploy when an airbag is deployed; a molded article obtained by molding the thermoplastic elastomer composition; and an instrument panel skin made of the thermoplastic elastomer composition. [Means for solving the problem]

[0007] As a result of intensive investigations aimed at solving the above-mentioned problems, the present inventors have found that a thermoplastic elastomer composition obtained by mixing an ethylene-propylene-non-conjugated diene copolymer rubber, an olefin-based resin, and a hydrocarbon-based rubber softener with a specific content of a hydrogenated copolymer of a vinyl aromatic compound and a conjugated diene having specific thermal properties, and crosslinking the mixture with a crosslinking agent, can achieve both easy breakability and excellent flexibility over a wide temperature range, and when used as an instrument panel skin, the skin can be easily deployed when an airbag is deployed, and a molded article obtained by molding the thermoplastic elastomer composition, and an instrument panel skin made of the thermoplastic elastomer composition, thereby completing the present invention. That is, the present invention has the following features.

[0008] [1] A thermoplastic elastomer composition comprising the following components (a) to (d), containing 1 to 20 mass% of component (c) relative to 100 mass% of the total of components (a) to (d), and crosslinked with the following component (e): Component (a): Ethylene-propylene-non-conjugated diene copolymer rubber Component (b): Olefin resin Component (c): A hydrogenated copolymer of a vinyl aromatic compound and a conjugated diene having a glass transition temperature of 0°C or higher. Component (d): Hydrocarbon-based rubber softener Component (e): Crosslinking agent

[0009] [2] The thermoplastic elastomer composition according to [1], wherein, when the component (a) is a non-oil-extended ethylene-propylene-non-conjugated diene copolymer rubber, the weight average molecular weight is 100,000 or more and less than 300,000, and when the component (a) is an oil-extended ethylene-propylene-non-conjugated diene copolymer rubber, the weight average molecular weight is 300,000 or more and 1,000,000 or less.

[0010] [3] The thermoplastic elastomer composition according to [1] or [2], containing 10 to 79 mass% of the component (d) relative to 100 mass% in total of the components (a) to (d).

[0011] [4] A molded article of the thermoplastic elastomer composition according to any one of [1] to [3].

[0012] [5] The molded article according to [4], which is obtained by injection molding.

[0013] [6] The molded article according to [4], which is obtained by extrusion molding.

[0014] [7] A skin for an instrument panel, comprising the thermoplastic elastomer composition according to any one of [1] to [3].

[0015] [8] The instrument panel skin according to [7], which is provided with an airbag mechanism. Effect of the Invention

[0016] The thermoplastic elastomer composition of the present invention combines ease of breaking over a wide temperature range with excellent flexibility. Therefore, a molded article obtained by molding the thermoplastic elastomer composition of the present invention, in particular an instrument panel skin made of the thermoplastic elastomer composition of the present invention, is excellent in safety because the skin easily deploys over a wide temperature range when an airbag is deployed, and an instrument panel skin suitable for applications requiring flexibility can be obtained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The following describes in detail an embodiment of the present invention. However, the description of the components described below is an example of an embodiment of the present invention, and the present invention is not limited to the following content as long as it does not exceed the gist of the present invention. In this specification, when the expression "to" is used, it is intended to include the numerical values ​​or physical property values ​​written before and after it. In addition, numerical values ​​or physical property values ​​written as upper and lower limits are intended to include those values.

[0018] [Thermoplastic elastomer composition] The thermoplastic elastomer composition of the present invention contains the following components (a) to (d), and contains 1 to 20 mass% of component (c) relative to 100 mass% in total of components (a) to (d). The thermoplastic elastomer composition is crosslinked in the presence of the following component (e). Component (a): Ethylene-propylene-non-conjugated diene copolymer rubber Component (b): Olefin resin Component (c): A hydrogenated copolymer of a vinyl aromatic compound and a conjugated diene having a glass transition temperature of 0°C or higher. Component (d): Hydrocarbon-based rubber softener Component (e): Crosslinking agent

[0019] In the thermoplastic elastomer composition of the present invention, by using the component (c) in a specified ratio, it is possible to improve the ease of breaking in a lower temperature range while maintaining flexibility.

[0020] [Component (a): Ethylene-propylene-non-conjugated diene copolymer rubber] The ethylene-propylene-non-conjugated diene copolymer rubber of component (a) used in the present invention is a copolymer rubber containing ethylene, propylene, and a non-conjugated diene compound as copolymerization components. The ethylene-propylene-non-conjugated diene copolymer rubber includes an oil-extended type which is a mixture of an ethylene-propylene-non-conjugated diene copolymer rubber and a hydrocarbon-based rubber softener (hereinafter, also referred to as "oil-extended ethylene-propylene-non-conjugated diene copolymer rubber"), and a non-oil-extended type which does not contain a hydrocarbon-based rubber softener. In this embodiment, it is preferable to include the non-oil-extended type, but the oil-extended type can also be suitably used. That is, in the present invention, the ethylene-propylene-non-conjugated diene copolymer rubber of component (a) may be either an oil-extended type or a non-oil-extended type, and either a non-oil-extended type or an oil-extended type may be used alone, or two or more types may be used in any combination and ratio, or one or more types of oil-extended type and one or more types of non-oil-extended type may be used in any combination and ratio. As described later, the ease of breakage can be further improved by combining oil-extended ethylene-propylene-non-conjugated diene copolymer rubber and non-oil-extended ethylene-propylene-non-conjugated diene copolymer rubber in a specific ratio. In addition, when component (a) is an oil-extended ethylene-propylene-non-conjugated diene copolymer rubber, the hydrocarbon-based rubber softener contained in this oil-extended ethylene-propylene-non-conjugated diene copolymer rubber is included in the hydrocarbon-based rubber softener as component (d).

[0021] The non-conjugated diene units in the ethylene-propylene-non-conjugated diene copolymer rubber of component (a) include dicyclopentadiene units, 1,4-hexadiene units, cyclooctadiene units, methylenenorbornene units, ethylidenenorbornene units, vinylidenenorbornene units, etc. Among these, the ethylidenenorbornene units and / or vinylidenenorbornene units are preferably contained because they can provide the ethylene-propylene-non-conjugated diene copolymer rubber with a suitable crosslinking structure. The non-conjugated diene units listed above can be used alone or in any combination and ratio of two or more of them.

[0022] The content of ethylene units in the ethylene-propylene-non-conjugated diene copolymer rubber is not particularly limited, but is preferably 50% by mass or more, more preferably 55% by mass or more, and even more preferably 60% by mass or more, based on 100% by mass of the total monomer units constituting component (a). On the other hand, it is preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 80% by mass or less. When the content of ethylene units is within the above range, it is easy to impart appropriate flexibility.

[0023] The content of the propylene unit in the ethylene-propylene-non-conjugated diene copolymer rubber is preferably 9% by mass or more, more preferably 12% by mass or more, based on 100% by mass of the total of the monomer units constituting the component (a). On the other hand, it is preferably 45% by mass or less, more preferably 37% by mass or less. When the content of the propylene unit is within the above range, it is easy to impart appropriate flexibility.

[0024] Furthermore, the content of the non-conjugated diene unit in the ethylene-propylene-non-conjugated diene copolymer rubber is preferably 1% by mass or more, more preferably 3% by mass or more, based on 100% by mass of the total monomer units constituting component (a). On the other hand, it is preferably 10% by mass or less, more preferably 8% by mass or less. If the content of the non-conjugated diene unit is equal to or more than the lower limit, it is preferable from the viewpoint of increasing the degree of crosslinking of the thermoplastic elastomer composition, and if it is equal to or less than the upper limit, it is preferable from the viewpoint of moldability.

[0025] The content of each structural unit in the ethylene-propylene-non-conjugated diene copolymer rubber can be determined by infrared spectroscopy.

[0026] Of the components (a), the weight average molecular weight of the non-oil-extended ethylene-propylene-non-conjugated diene copolymer rubber, calculated as polypropylene by gel permeation chromatography (GPC), is preferably less than 300,000, more preferably less than 280,000, and even more preferably less than 250,000, from the viewpoint of suppressing the generation of foreign matter and improving the appearance of the resulting molded article. Also, from the viewpoint of the design of the extrusion molded article, it is preferably 100,000 or more, more preferably 120,000 or more, and even more preferably 150,000 or more. On the other hand, the weight average molecular weight of the oil-extended ethylene-propylene-non-conjugated diene copolymer rubber, calculated as polypropylene by the GPC method, is preferably 300,000 or more, more preferably 350,000 or more, and even more preferably 400,000 or more from the viewpoint of preventing bleeding out of the hydrocarbon-based rubber softener. Also, from the viewpoint of the appearance of the obtained molded article, it is preferably 1,000,000 or less, more preferably 900,000 or less, and even more preferably 800,000 or less.

[0027] The conditions for measuring the weight average molecular weight of the ethylene-propylene-non-conjugated diene copolymer rubber in component (a) by GPC method are as follows. Equipment: Waters liquid chromatogram RI detector "WATERS150C" Column: Shodex AD806MS x 3 (8.0 mm inner diameter x 300 mm length) Detector: IR (dispersive, 3.42 μm) Solvent: orthodichlorobenzene Temperature: 140℃ Flow rate: 1.0mL / min Injection volume: 200μL Concentration: 10mg / mL Calibration sample: Polydisperse standard polyethylene Calibration method: Polypropylene conversion using the Mark-Houwink formula

[0028] Hydrocarbon-based rubber softeners used in oil-extended ethylene-propylene-non-conjugated diene copolymer rubber include mineral oil-based softeners and synthetic resin-based softeners, but mineral oil-based softeners are preferred from the viewpoint of affinity with other components. Mineral oil-based softeners are generally mixtures of aromatic hydrocarbons, naphthenic hydrocarbons, and paraffinic hydrocarbons, and those in which 50% or more of the total carbon atoms are paraffinic hydrocarbons are called paraffinic oils, those in which 30-45% of the total carbon atoms are naphthenic hydrocarbons, and those in which 35% or more of the total carbon atoms are aromatic hydrocarbons are called aromatic oils. Among these, paraffinic oils are preferred. The hydrocarbon-based rubber softeners can be used alone or in any combination and ratio of two or more types.

[0029] In the oil-extended ethylene-propylene-non-conjugated diene copolymer rubber, the content ratio of the ethylene-propylene-non-conjugated diene copolymer rubber to the hydrocarbon-based rubber softener, expressed as [mass of the ethylene-propylene-non-conjugated diene copolymer rubber] / [mass of the hydrocarbon-based rubber softener part], is usually 100 / 10 to 150, and preferably 100 / 20 to 120.

[0030] The ethylene-propylene-non-conjugated diene copolymer rubber of component (a) can be produced by a polymerization method using a known olefin polymerization catalyst, for example, a slurry polymerization method, a solution polymerization method, a bulk polymerization method, or a gas phase polymerization method using a Ziegler-Natta catalyst, a metallocene complex, or a nonmetallocene complex.

[0031] Among the ethylene-propylene-non-conjugated diene copolymer rubbers of component (a) used in the present invention, the Mooney viscosity (ML 1+4 , 125° C.) is usually 10 to 100 or less, and preferably 15 to 95. On the other hand, the Mooney viscosity (ML 1+4 , 125° C.) is usually 20 to 100 or less, and preferably 30 to 90. When the Mooney viscosity of the ethylene-propylene-non-conjugated diene copolymer rubber of component (a) is not less than the above lower limit, the appearance of the obtained molded article is good, and when it is not more than the above upper limit, the moldability is good.

[0032] A known method can be used for producing oil-extended ethylene-propylene-non-conjugated diene copolymer rubber (oil extension method), for example, a method of mechanically kneading ethylene-propylene-non-conjugated diene copolymer rubber and a hydrocarbon-based rubber softener using a mixing roll or Banbury mixer to extend the rubber, a method of adding a predetermined amount of a hydrocarbon-based rubber softener to ethylene-propylene-non-conjugated diene copolymer rubber and then removing the solvent by a method such as steam stripping, and a method of stirring a mixture of crumb-like ethylene-propylene-non-conjugated diene copolymer rubber and a hydrocarbon-based rubber softener with a Henschel mixer to impregnate the mixture.

[0033] The ethylene-propylene-non-conjugated diene copolymer rubber of component (a) is commercially available. Examples of non-oil-extended ethylene-propylene-non-conjugated diene copolymer rubber include JSR EPR manufactured by JSR Corporation, Mitsui EPT manufactured by Mitsui Chemicals, Esprene (registered trademark) manufactured by Sumitomo Chemical Co., Ltd., Keltan (registered trademark) manufactured by LANXESS, Engage (registered trademark) manufactured by Dow, and Tafmer (registered trademark) manufactured by Mitsui Chemicals, Inc. Examples of oil-extended ethylene-propylene-non-conjugated diene copolymer rubbers include JSR EPR manufactured by JSR Corporation, Mitsui EPT manufactured by Mitsui Chemicals, Esprene (registered trademark) manufactured by Sumitomo Chemical Co., Ltd., Keltan (registered trademark) manufactured by ARLANXEO, NORDEL (registered trademark) manufactured by DOW CHEMICAL, and KEP manufactured by KUMHO POLYCHEM.

[0034] [Component (b): Olefin resin] In the thermoplastic elastomer composition of the present invention, the component (b) contributes to moldability. The olefin resin of component (b) used in the present invention is preferably a propylene resin, and is preferably a propylene resin having a propylene unit content of more than 50% by mass relative to the total monomer units, more preferably 60% by mass or more, even more preferably 75% by mass or more, and particularly preferably 90% by mass or more. When the propylene unit content of the propylene resin is equal to or more than the above lower limit, the heat resistance and rigidity tend to be good. On the other hand, the upper limit is not particularly limited and is usually 100% by mass. The propylene unit content of the propylene resin can be determined by infrared spectroscopy.

[0035] The type of the propylene-based resin of component (b) is not particularly limited, and any of propylene homopolymers, propylene random copolymers, propylene block copolymers, etc. can be used. The propylene-based resin of component (b) can be used alone or in any combination and ratio of two or more of these.

[0036] When component (b) is a propylene random copolymer, examples of the monomer copolymerized with propylene include ethylene, 1-butene, 2-methylpropylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, and 1-octene. When component (b) is a propylene block copolymer, examples include propylene block copolymers obtained by multi-stage polymerization, more specifically, propylene block copolymers obtained by polymerizing polypropylene in the first stage and polymerizing a propylene-ethylene copolymer in the second stage.

[0037] The melt flow rate (MFR) of component (b) at 230°C and a load of 21.2 N is usually 0.05 g / 10 min or more, and from the viewpoint of fluidity, it is preferably 0.1 g / 10 min or more, and more preferably 0.5 g / 10 min or more. On the other hand, the MFR of component (b) is usually 100 g / 10 min or less, and from the viewpoint of moldability, it is preferably 70 g / 10 min or less, more preferably 50 g / 10 min or less, and from the viewpoint of fragility, it is further preferably 30 g / 10 min or less, and particularly preferably 10 g / 10 min or less.

[0038] The propylene-based resin of component (b) can be produced by a polymerization method using a known olefin polymerization catalyst. For example, a multi-stage polymerization method using a Ziegler-Natta catalyst can be used. For this multi-stage polymerization method, a slurry polymerization method, a solution polymerization method, a bulk polymerization method, a gas phase polymerization method, etc. can be used, and two or more of these methods can be combined to produce the resin.

[0039] In addition, the propylene-based resin of component (b) may be a commercially available product. Commercially available propylene-based resins can be procured from the manufacturers listed below and can be appropriately selected. Available commercially include PrimPolypro (registered trademark) from Prime Polymer, Sumitomo Noblen (registered trademark) from Sumitomo Chemical, polypropylene block copolymer from SunAllomer, Novatec (registered trademark) PP from Japan Polypropylene, Moplen (registered trademark) from LyondellBasell, ExxonMobil PP from ExxonMobil, Formolene (registered trademark) from Formosa Plastics, Borealis PP from Borealis, SEETEC PP from LG Chemical, ASIPOLYPROPYLENE from A. Schulman, INEOS PP from INEOS Olefins & Polymers, Braskem PP from Braskem, Samsung Total from SAMSUNG TOTAL PETROCHEMICALS, Sabic (registered trademark) PP from Sabic, TOTAL PETROCHEMICALS from TOTAL PETROCHEMICALS, and YUPLENE (registered trademark) from SK.

[0040] [Component (c): A hydrogenated copolymer of a vinyl aromatic compound and a conjugated diene having a glass transition temperature of 0°C or higher] Component (c) used in the thermoplastic elastomer composition of the present invention is a hydrogenated copolymer of a vinyl aromatic compound and a conjugated diene (hereinafter, sometimes referred to as a "hydrogenated copolymer") having a glass transition temperature of 0°C or higher. By making the glass transition temperature of component (c) 0°C or higher, it is possible to improve the ease of breaking in the low temperature range while maintaining flexibility. From the viewpoint of tensile properties at low temperatures, the lower limit of the glass transition temperature of component (c) is preferably 10°C or higher. From the viewpoint of tensile properties at room temperature, the upper limit is preferably 40°C or lower, more preferably 30°C or lower.

[0041] The glass transition temperature of the component (c) can be measured under the following measurement conditions and by the following measurement method, with reference to JIS K6394. <Measurement conditions> Measurement equipment: TA Instruments dynamic viscoelasticity measuring device "RSA-III" Measurement mode: Tensile Atmosphere: Nitrogen Temperature: -20~100℃ Heating rate: 2℃ / min Soak time: 30 seconds Frequency: 1Hz

[0042] <Measurement method> The component (c) is press-molded at 200° C. into a flat plate having a thickness of 1 mm, which is then cut into a rectangular piece having a width of 4 mm, which is then fixed to the measuring device and measured under the measuring conditions described above.

[0043] The hydrogenated copolymer of a vinyl aromatic compound and a conjugated diene of component (c) is preferably a hydrogenated copolymer consisting of a polymer block A of a vinyl aromatic compound constituting a hard segment and a copolymer block B of a vinyl aromatic compound and a conjugated diene constituting a soft segment.

[0044] Examples of the vinyl aromatic compound of the polymer block A include styrene compounds such as styrene, α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, and 1,3-dimethylstyrene, and polycyclic aromatic compounds such as vinylnaphthalene and vinylanthracene. Of these, styrene compounds are preferred, and styrene is particularly preferred.

[0045] The vinyl aromatic compound used in the copolymer block B may be the same as the vinyl aromatic compound used in the polymer block A.

[0046] Conjugated dienes used in the copolymer block B include, for example, butadiene, isoprene, 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene. Of these, butadiene, isoprene, or a mixture of butadiene and isoprene is preferred, with butadiene being particularly preferred.

[0047] Moreover, polymer block B is preferably a random copolymer block in order to impart flexibility to the resulting thermoplastic elastomer composition.

[0048] Component (c) is a hydrogenated block copolymer obtained by hydrogenating the carbon-carbon double bonds derived from the conjugated diene of the block copolymer, and may be either completely hydrogenated (fully hydrogenated) or partially hydrogenated (selectively hydrogenated).

[0049] The content of polymer block A in the block copolymer of component (c) is usually 3% by mass or more and 70% by mass or less. When the content of polymer block A is equal to or more than the above lower limit, the thermoplastic elastomer composition tends to have excellent mechanical strength and heat resistance. The lower limit of the content of polymer block A is preferably 4% by mass or more, more preferably 5% by mass or more. On the other hand, the upper limit of the content of polymer block A is preferably 50% by mass or less, more preferably 30% by mass or less. When the content of polymer block A is equal to or less than the above upper limit, flexibility can be maintained and bleeding of the hydrocarbon rubber softener can be suppressed.

[0050] The proportion of the constituent units derived from the vinyl aromatic compound in the hydrogenated copolymer of component (c) is usually 50% by mass or more and 80% by mass or less. From the viewpoint of improving the scratch resistance of the thermoplastic elastomer composition, the lower limit of the proportion of the constituent units derived from the vinyl aromatic compound is preferably 55% by mass or more, and the upper limit is preferably 75% by mass or less. Therefore, it is preferable that the proportion of the constituent units derived from a vinyl aromatic compound in polymer block B, in total with the constituent units derived from a vinyl aromatic compound in polymer block A, is such that the proportion of the constituent units derived from a vinyl aromatic compound in component (c) falls within the above-mentioned range.

[0051] The weight average molecular weight of the block copolymer of component (c) measured by the GPC method in terms of polystyrene is preferably 50,000 or more, more preferably 75,000 or more, as a lower limit from the viewpoint of improving the mechanical strength of the thermoplastic elastomer composition, and is preferably 1,000,000 or less, more preferably 500,000 or less, as an upper limit from the viewpoint of moldability.

[0052] The block copolymer of component (c) can be produced by any known method. For example, a method of block polymerization in an inert solvent using a lithium catalyst or the like (see JP-B-40-23798, etc.) can be mentioned. In addition, the hydrogenation treatment of the block copolymer can be carried out in an inert solvent in the presence of a hydrogenation catalyst (see JP-B-42-8704, JP-B-43-6636, JP-A-59-133203, JP-A-60-79005, etc.). In addition, the hydrogenated copolymer of component (c) can be a commercially available product. An example of a commercially available hydrogenated copolymer is "Tuftec (registered trademark) SOE-SS" (manufactured by Asahi Kasei Corporation).

[0053] The hydrogenated copolymer of a vinyl aromatic compound and a conjugated diene as component (c) may be used alone or in any combination and ratio of two or more kinds.

[0054] [Component (d): Hydrocarbon-based rubber softener] The thermoplastic elastomer composition of the present invention contains a hydrocarbon-based rubber softener as component (d) in order to soften the resulting thermoplastic elastomer composition and increase its flexibility and elasticity, as well as to improve the processability and flowability of the resulting thermoplastic elastomer composition.

[0055] The hydrocarbon rubber softener of component (d) can be the same as the hydrocarbon rubber softener contained in the oil-extended ethylene-propylene-non-conjugated diene copolymer rubber of component (a). However, the hydrocarbon rubber softener contained in the oil-extended ethylene-propylene-non-conjugated diene copolymer rubber and the hydrocarbon rubber softener added as component (d) do not have to be the same, and may be different.

[0056] The kinetic viscosity of the hydrocarbon rubber softener of component (d) at 40°C is preferably 20 centistokes (cSt) or more, more preferably 50 cSt or more, and is preferably 800 cSt or less, more preferably 600 cSt or less. The flash point (COC method) of the hydrocarbon rubber softener is preferably 200°C or more, more preferably 250°C or more.

[0057] The hydrocarbon-based rubber softeners of component (d) may be used alone or in any combination and ratio of two or more kinds.

[0058] [Component (e): Crosslinking agent] The thermoplastic elastomer composition of the present invention is crosslinked with a crosslinking agent of component (e). In the thermoplastic elastomer composition of the present invention, the crosslinking agent of component (e) acts as a crosslinking agent in dynamic heat treatment. As the crosslinking agent of component (e), an organic peroxide, a crosslinking assistant, etc. can be used. These crosslinking agents may be used alone or in combination of two or more.

[0059] As the organic peroxide, either an aromatic organic peroxide or an aliphatic organic peroxide can be used. Specific examples of the peroxides include dialkyl peroxides such as di-t-butyl peroxide, t-butylcumyl peroxide, dicumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, 2,5-dimethyl-2,5-di(t-butylperoxy)-3-hexyne, 1,3-bis(t-butylperoxyisopropyl)benzene, and 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane; peroxy esters such as t-butyl peroxybenzoate, t-butylperoxyisopropyl carbonate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, and 2,5-dimethyl-2,5-di(benzoylperoxy)-3-hexyne; and hydroperoxides such as acetyl peroxide, lauroyl peroxide, benzoyl peroxide, p-chlorobenzoyl peroxide, and 2,4-dichlorobenzoyl peroxide. Among these, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane is preferred. The organic peroxides listed above may be used alone or in combination of two or more.

[0060] When producing the thermoplastic elastomer composition of the present invention, it is preferable to carry out a dynamic heat treatment in the presence of the organic peroxide and a crosslinking aid.

[0061] Examples of the crosslinking aid include peroxide aids such as sulfur, p-quinone dioxime, p-dinitrosobenzene, and 1,3-diphenyl guanidine; polyfunctional vinyl compounds such as divinylbenzene, triallyl cyanurate, triallyl isocyanurate, and diallyl phthalate; and polyfunctional (meth)acrylate compounds such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and allyl (meth)acrylate. These may be used alone or in combination of two or more.

[0062] [Mixing ratio] The blending ratio of the raw materials of the thermoplastic elastomer composition of the present invention will be described below. The thermoplastic elastomer composition of the present invention is a thermoplastic elastomer composition obtained by crosslinking a composition containing components (a) to (d) in the presence of component (e), preferably by dynamic heat treatment, and the blending ratio of each component described below means the amount charged before dynamic heat treatment.

[0063] The content of component (a) is preferably 10% by mass or more, more preferably 15% by mass or more, based on the total of components (a) to (d) (100% by mass), from the viewpoint of flexibility, and is preferably 40% by mass or less, more preferably 35% by mass or less, from the viewpoint of moldability.

[0064] The content of component (b) is preferably 10% by mass or more, based on the total of components (a) to (d) (100% by mass), from the viewpoint of moldability, while it is preferably 30% by mass or less, more preferably 25% by mass or less, from the viewpoint of flexibility.

[0065] The content of component (c) is 1% by mass or more, and preferably 4% by mass or more, based on the total of components (a) to (d) (100% by mass) from the viewpoint of breakability, while it is 20% by mass or less from the viewpoint of flexibility.

[0066] The content of component (d) is preferably 10% by mass or more, more preferably 20% by mass or more, based on 100% by mass of the total of components (a) to (d). On the other hand, it is preferably 79% by mass or less, more preferably 60% by mass or less. When the content of component (d) is equal to or more than the lower limit, flexibility and moldability tend to be good, and when it is equal to or less than the upper limit, molding tends to be easy. When an oil-extended ethylene-propylene-non-conjugated diene copolymer rubber is used as component (a), as described above, the hydrocarbon-based rubber softener in component (a) is included in the hydrocarbon-based rubber softener as component (d).

[0067] The amount of the organic peroxide used as component (e) is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.3 parts by mass or more, based on 100 parts by mass of the total of components (a) to (d) in order to sufficiently proceed with the crosslinking reaction, while from the viewpoint of controlling the crosslinking reaction, it is preferably 5.0 parts by mass or less, more preferably 4.0 parts by mass or less, and even more preferably 3.0 parts by mass or less.

[0068] The amount of the crosslinking aid used as component (e) is usually within the range of 0.01 to 4.0 parts by mass, and preferably 0.05 to 3.0 parts by mass, per 100 parts by mass of the total of components (a) to (d). If it is equal to or more than the lower limit, the effect of using the crosslinking aid can be obtained, and if it is equal to or less than the upper limit, it is preferable from the viewpoint of cost.

[0069] When an oil-extended ethylene-propylene-non-conjugated diene copolymer rubber and a non-oil-extended ethylene-propylene-non-conjugated diene copolymer rubber are used in combination as component (a), the mass ratio of the oil-extended ethylene-propylene-non-conjugated diene copolymer rubber to the non-oil-extended ethylene-propylene-non-conjugated diene copolymer rubber is preferably 1:0.1 to 10, more preferably 1:0.2 to 8, even more preferably 1:0.5 to 5, and particularly preferably 1:0.7 to 4. By using the oil-extended ethylene-propylene-non-conjugated diene copolymer rubber and the non-oil-extended ethylene-propylene-non-conjugated diene copolymer rubber in this mass ratio in combination, the product tends to have particularly excellent breakability.

[0070] [Other ingredients] In addition to the above-mentioned components (a) to (e), other components may be blended into the thermoplastic elastomer composition of the present invention depending on the purpose, provided that the effects of the present invention are not impaired.

[0071] Examples of other components include various additives such as fillers, antioxidants, heat stabilizers, light stabilizers, ultraviolet absorbers, neutralizing agents, lubricants, antifogging agents, antiblocking agents, slip agents, dispersants, colorants, flame retardants, antistatic agents, conductivity imparting agents, metal deactivators, molecular weight regulators, antibacterial agents, antifungal agents, fluorescent whitening agents, etc., thermoplastic resins other than components (a) to (c), elastomers other than components (a) to (c), etc. Any of these may be used alone or in combination.

[0072] Examples of the filler include glass fiber, hollow glass spheres, carbon fiber, talc, calcium carbonate, mica, potassium titanate fiber, silica, metal soap, titanium dioxide, carbon black, etc. When a filler is used, it is usually used in an amount of 0.1 to 50 parts by mass per 100 parts by mass of the total of the components (a) to (d).

[0073] Examples of the antioxidant include phenol-based antioxidants, phosphite-based antioxidants, thioether-based antioxidants, etc. When an antioxidant is used, it is usually used in an amount of 0.01 to 3.0 parts by mass per 100 parts by mass of the total of the components (a) to (d).

[0074] Examples of thermoplastic resins other than components (a) to (c) include polyphenylene ether resins; polyamide resins such as nylon 6 and nylon 66; polyester resins such as polyethylene terephthalate and polybutylene terephthalate; polyoxymethylene resins such as polyoxymethylene homopolymers and polyoxymethylene copolymers; polymethyl methacrylate resins, and olefin resins (excluding those corresponding to components (a) and (b)). Examples of elastomers other than components (a) to (c) include styrene elastomers such as styrene-butadiene copolymer rubber and styrene-isoprene copolymer rubber (excluding those corresponding to component (c)); polyester elastomers; and polybutadiene.

[0075] [Method of producing thermoplastic elastomer composition] The thermoplastic elastomer composition of the present invention is preferably one obtained by crosslinking the components (a) to (d) at a predetermined content ratio by dynamic heat treatment in the presence of the component (e).

[0076] In the present invention, "dynamic heat treatment" means kneading in a molten or semi-molten state. This dynamic heat treatment is preferably performed by melt kneading, and as a mixing and kneading device for this purpose, for example, a non-open type Banbury mixer, a mixing roll, a kneader, or a twin-screw extruder is used. Among these, it is preferable to use a twin-screw extruder. In a preferred embodiment of the production method using this twin-screw extruder, each component is supplied to a raw material supply port (hopper) of a twin-screw extruder having multiple raw material supply ports, and dynamic heat treatment is performed.

[0077] The temperature when the dynamic heat treatment is carried out is usually 80 to 300° C., and preferably 100 to 250° C. The time for which the dynamic heat treatment is carried out is usually 0.1 to 30 minutes.

[0078] When the thermoplastic elastomer composition of the present invention is subjected to dynamic heat treatment using a twin-screw extruder, it is preferable to extrude the composition while maintaining the relationship shown in the following formula among the barrel radius R (mm), screw rotation speed N (rpm), and discharge rate Q (kg / hour) of the twin-screw extruder, and it is more preferable to extrude the composition while maintaining the relationship shown in the following formula (2). 2.6 <NQ / R 3 <22.6(1) 3.0 <NQ / R 3 <20.0(2)

[0079] It is preferable that the above relationship between the barrel radius R (mm), screw rotation speed N (rpm), and discharge rate Q (kg / hour) of the twin-screw extruder is larger than the above lower limit value in order to efficiently produce the thermoplastic elastomer composition, while it is preferable that the above relationship is smaller than the above upper limit value in order to suppress heat generation due to shear and to prevent the generation of foreign matter that causes a defective appearance.

[0080] [Physical properties of thermoplastic elastomer composition] The thermoplastic elastomer composition of the present invention has excellent flexibility and excellent ease of breaking over a wide temperature range from low to high temperatures.

[0081] In the present invention, the value of the tensile strength at break measured by the method shown in the examples below is used as an index of fragility. Since it is preferable to have excellent fragility while maintaining strength, the value of the tensile strength at break is preferably less than 25.0 MPa, more preferably less than 20.0 MPa at -35°C. On the other hand, it is preferably 5.0 MPa or more. Furthermore, at 23°C, it is preferably less than 5.5 MPa, more preferably less than 5.0 MPa, even more preferably less than 4.5 MPa, on the other hand, it is preferably 2.0 MPa or more. Furthermore, at 85°C, it is preferably less than 2.7 MPa, more preferably less than 2.4 MPa, even more preferably less than 2.1 MPa, on the other hand, it is preferably 0.5 MPa or more.

[0082] The thermoplastic elastomer composition of the present invention preferably has a melt flow rate (MFR) of 0.5 to 200 g / 10 min at a temperature of 230° C. and a measuring load of 49 N according to JIS K7210 in order to provide excellent moldability. When the MFR of the thermoplastic elastomer composition is 0.5 g / 10 min or more, the flowability tends to be good, and when it is 200 g / 10 min or less, it is preferable because burrs and the like during molding can be easily suppressed. From the viewpoint of flowability, the MFR of the thermoplastic elastomer composition of the present invention is more preferably 1.0 g / 10 min or more, even more preferably 5.0 g / 10 min or more, and particularly preferably 10 g / 10 min or more. On the other hand, from the viewpoint of suppressing burrs and the like during injection molding, the MFR of the thermoplastic elastomer composition of the present invention is more preferably 150 g / 10 min or less, even more preferably 120 g / 10 min or less.

[0083] From the viewpoint of flexibility, the thermoplastic elastomer composition of the present invention preferably has a Duro A hardness value of 40 to 70, more preferably 40 to 60. The method for measuring Duro A hardness will be described later in the Examples.

[0084] [Molded objects / Applications] The thermoplastic elastomer composition of the present invention can be molded into a molded article by various molding methods usually used for thermoplastic elastomer compositions, such as injection molding, extrusion molding, blow molding, compression molding, etc., and among these, molded articles obtained by injection molding and extrusion molding are preferred. In addition, the composition can also be molded into a molded article by carrying out secondary processing such as lamination molding and thermoforming after the above molding.

[0085] The thermoplastic elastomer composition of the present invention has the above-mentioned effects and is therefore suitable as an instrument panel skin, particularly suitable as an instrument panel skin equipped with an airbag mechanism. The use of the thermoplastic elastomer composition of the present invention is not limited to instrument panel skin, but can be used in a wide range of fields, such as automobile parts (weather strips, ceiling materials, interior seats, bumper moldings, side moldings, air spoilers, air duct hoses, various packings, etc.), civil engineering and building material parts (waterstop materials, joint materials, window frames, etc.), sports goods (grip types for golf clubs and tennis rackets, etc.), industrial parts (hose tubes, gaskets, etc.), home appliance parts (hoses, packings, etc.), medical parts (medical containers, gaskets, packings, etc.), food parts (containers, packings, etc.), medical equipment parts, electric wires, miscellaneous goods, etc. EXAMPLES

[0086] The present invention will be described in more detail below using examples, but the present invention is not limited to the following examples as long as it does not exceed the gist of the invention. The values ​​of various production conditions and evaluation results in the following examples are meant as preferred upper or lower limit values ​​in the embodiment of the present invention, and the preferred range may be a range defined by a combination of the above-mentioned upper or lower limit values ​​and the values ​​of the following examples or values ​​of the examples.

[0087] [raw materials] The raw materials used in the following Examples and Comparative Examples are as follows.

[0088] <Component (a)> (a-1): Oil-extended ethylene-propylene-ethylidene norbornene copolymer rubber / JSR Corporation JSR EPR EP505EC Contains 100 parts by mass of paraffin oil for every 100 parts by mass of ethylene-propylene-ethylidene norbornene copolymer rubber. Mooney Viscosity (ML 1+4 ,125℃):65 Propylene unit content: 29.5% by mass Ethylene unit content: 66% by mass Ethylidene norbornene unit content: 4.5% by mass Weight average molecular weight converted to polypropylene (PP): 647,000 (a-2): Non-oil-extended ethylene-propylene-ethylidene norbornene copolymer rubber / Mitsui Chemicals, Inc. Mitsui EPT3092PM Mooney Viscosity (ML 1+4 ,125℃):57 Propylene unit content: 29.5% by mass Ethylene unit content: 66% by mass Ethylidene norbornene unit content: 4.5% by mass Weight average molecular weight converted to polypropylene (PP): 223,000

[0089] <Ingredient (b)> (b-1): Propylene-ethylene random copolymer / Novatec (registered trademark) EG8B manufactured by Japan Polypropylene Corporation MFR: 0.8g / 10min (measurement conditions: 230℃, load 21.2N)

[0090] <Ingredient (c)> (c-1): Hydrogenated block copolymer consisting of polymer block A of vinyl aromatic compound constituting the hard segment and copolymer block B of vinyl aromatic compound and conjugated diene constituting the soft segment / Tuftec (registered trademark) SOE-SS "S1605" manufactured by Asahi Kasei Corporation Hydrogenation: Fully hydrogenated Glass transition temperature: 16℃ Polymer block: styrene Copolymer block B: styrene and butadiene Styrene unit content: 60% by mass Weight average molecular weight: 203,000 (c-2): Hydrogenated block copolymer consisting of polymer block A of vinyl aromatic compound constituting the hard segment and copolymer block B of vinyl aromatic compound and conjugated diene constituting the soft segment / Tuftec (registered trademark) SOE-SS "S1609" manufactured by Asahi Kasei Corporation Hydrogenation: Selective hydrogenation Glass transition temperature: 17℃ Polymer block A: styrene Copolymer block B: styrene and butadiene Weight average molecular weight; 203,000 (c'-1): Hydrogenated block copolymer consisting of polymer block A of vinyl aromatic compound constituting the hard segment and copolymer block B of vinyl aromatic compound and conjugated diene constituting the soft segment / Tuftec (registered trademark) SOE-SS "S1606" manufactured by Asahi Kasei Corporation Hydrogenation: Fully hydrogenated Glass transition temperature: -15℃ Polymer block A: styrene Copolymer block B: styrene and butadiene Weight average molecular weight; 150,000 (c'-2): Hydrogenated block copolymer consisting of polymer block A of vinyl aromatic compound constituting hard segment and polymer block B of conjugated diene constituting soft segment / Kraton G "G1657" manufactured by Kraton Corporation Hydrogenation: Fully hydrogenated Glass transition temperature: -57℃ Polymer block A: styrene Polymer block B: butadiene Polymer block A content: 13% by mass Weight average molecular weight; 109,000

[0091] <Ingredient (d)> (d-1): Paraffin-based oil / Idemitsu Kosan Co., Ltd. Diana (registered trademark) Process Oil PW-90 Kinematic viscosity at 40℃: 95.54cSt Flash point: 272℃

[0092] <Ingredient (e)> (e-1): A mixture of 40% by mass of 2,5-dimethyl-2,5-di(t-butylperoxy)hexane and 60% by mass of calcium carbonate / Trigonox 101-40C manufactured by Nouryon Chemical Co., Ltd. (e-2): Trimethylolpropane trimethacrylate / Mitsubishi Chemical Corporation Acrylatester TMP

[0093] [Evaluation method] The thermoplastic elastomer compositions in the following Examples and Comparative Examples were evaluated as follows.

[0094] (1) Melt flow rate (MFR) The measurement was performed in accordance with the JIS K7210 standard at a measurement temperature of 230°C and a measurement load of 49N.

[0095] (2) Hardness: Duro A The mixture was injection molded using an in-line screw type injection molding machine (Toshiba Machine Co., Ltd. "IS130") under conditions of injection pressure of 50 MPa, cylinder temperature of 220°C, and mold temperature of 40°C to obtain a sheet with a width of 120 mm, length of 80 mm, and thickness of 2 mm. The hardness of the sheet was measured in accordance with ISO 7619.

[0096] (3) Tensile strength at break Using a Labo Plastomill (Toyo Seiki Co., Ltd., "4C150") at 180°C, an extruded sheet with a thickness of 0.5 mm was prepared and punched into a dumbbell-shaped test piece for measurement. The tensile strength at break was measured in a thermostatic bath at temperatures of -20°C, 23°C, and 85°C, with reference to JIS K6251 (JIS No. 3 dumbbell, tensile speed 500 mm / min). The smaller the tensile strength at break, the better it was, and it was evaluated according to the following criteria. <Temperature:-35℃> ◎: 5.0MPa or more and less than 20.0MPa ○: 20.0MPa or more and less than 25.0MPa △: 25.0MPa or more and less than 30.0MPa ×: 30.0MPa or more or less than 5.0MPa <Temperature: 23℃> ◎: 2.0MPa or more and less than 4.5MPa ○: 4.5MPa or more and less than 5.5MPa △: 5.5MPa or more and less than 6.0MPa ×: 6.0 MPa or more or less than 2.0 MPa <Temperature: 85℃> ◎: 0.5MPa or more and less than 2.1MPa ○: 2.1MPa or more and less than 2.4MPa △: 2.4MPa or more and less than 2.7MPa ×: 2.7MPa or more or less than 0.5MPa

[0097] [Examples / Comparative Examples] <Example 1> Component (a-1) (as the amount of ethylene-propylene-ethylidene norbornene copolymer rubber only excluding paraffinic oil) 29% by mass, component (a-2) 10% by mass, component (b-1) 12% by mass, component (c-1) 5% by mass, component (d-1) (as the total amount of paraffinic oil in component (a-1)) 44% by mass, 0.7 parts by mass of component (e-1) and 0.7 parts by mass of component (e-2) per 100 parts by mass of the total were fed from the feed port using an intermeshing mixer (Toyo Seiki Seisakusho "20C-200", mixer "R-60H"), and the mixture was heated to a temperature range of 180 to 190 ° C. and melt-kneaded for 5 minutes to produce a thermoplastic elastomer composition. The results of evaluation of the obtained thermoplastic elastomer composition are shown in Table 1.

[0098] <Examples 2 to 4 and Comparative Examples 1 to 6> Thermoplastic elastomer compositions were obtained in the same manner as in Example 1, except that the blending composition was changed as shown in Table 1. The obtained thermoplastic elastomer compositions were evaluated in the same manner as in Example 1, and the results are shown in Table 1.

[0099] [Table 1]

[0100] <Evaluation Results> As shown in Table 1, Examples 1 to 4 are excellent in flexibility and ease of breaking in the temperature ranges of -35°C, 23°C, and 85°C. On the other hand, Comparative Example 1 is an example in which component (c) was not used, and Comparative Examples 2 to 6 are examples in which a hydrogenated copolymer of a vinyl aromatic compound and a conjugated diene, which has a glass transition temperature of less than 0°C, was used. Each of these examples had good flexibility but poor ease of breaking, especially at -35°C. [Industrial Applicability]

[0101] The thermoplastic elastomer composition of the present invention has excellent flexibility and excellent breakability in a wide temperature range from low to high. Therefore, it is suitable as an instrument panel skin, and is particularly suitable as an instrument panel skin equipped with an airbag mechanism. The use of the thermoplastic elastomer composition of the present invention is not limited to instrument panel skin, but can be used in a wide range of fields such as automobile parts (weather strips, ceiling materials, interior seats, bumper moldings, side moldings, air spoilers, air duct hoses, various packings, etc.), civil engineering and building material parts (waterstop materials, joint materials, window frames, etc.), sporting goods (grip types for golf clubs and tennis rackets, etc.), industrial parts (hose tubes, gaskets, etc.), home appliance parts (hoses, packings, etc.), medical parts (medical containers, gaskets, packings, etc.), food parts (containers, packings, etc.), medical equipment parts, electric wires, miscellaneous goods, etc.

Claims

1. A thermoplastic elastomer composition comprising the following components (a) to (d), containing 1 to 20 mass% of component (c) relative to 100 mass% of the total of components (a) to (d), and crosslinked with the following component (e): Component (a): Ethylene-propylene-non-conjugated diene copolymer rubber Component (b): Olefin resin Component (c): A hydrogenated copolymer of a vinyl aromatic compound and a conjugated diene having a glass transition temperature of 0° C. or higher and 40° C. or lower. Component (d): Hydrocarbon-based rubber softener Component (e): Dialkyl peroxides and a crosslinking agent which is a crosslinking assistant

2. The thermoplastic elastomer composition according to claim 1, wherein when the component (a) is a non-oil-extended ethylene-propylene-non-conjugated diene copolymer rubber, the weight average molecular weight is 100,000 or more and less than 300,000, and when the component (a) is an oil-extended ethylene-propylene-non-conjugated diene copolymer rubber, the weight average molecular weight is 300,000 or more and 1,000,000 or less.

3. The thermoplastic elastomer composition according to claim 1 or 2, comprising 10 to 79 mass% of the component (d) relative to 100 mass% in total of the components (a) to (d).

4. A molded article of the thermoplastic elastomer composition according to any one of claims 1 to 3.

5. The molded article according to claim 4, which is obtained by injection molding.

6. The molded article according to claim 4, which is obtained by extrusion molding.

7. A skin for an instrument panel, comprising the thermoplastic elastomer composition according to any one of claims 1 to 3.

8. 8. The instrument panel skin according to claim 7, further comprising an airbag mechanism.

Citation Information

Patent Citations

  • Hydrogenated block copolymer elastomer composition

    JP1994116474A

  • Air-bag housing cover

    JP1996034304A

  • Production of thermoplastic elastomer for air bag covering material

    JP1996059895A

  • Air bag cover

    JP1998129387A

  • Resin composition

    JP2006291135A