Polymer composition for lamination and laminate using same

A novel ethylene-based ionomer with a linear structure addresses the limitations of conventional resins by enhancing heat-sealing and hot tack strength, enabling faster and more efficient packaging processes with reduced material thickness.

JP7567225B2Active Publication Date: 2024-10-16JAPAN POLYETHYLENE CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020107637
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-24
Filing Date
2020-06-23
Publication Date
2024-10-16
Estimated Expiration
2040-06-23

AI Technical Summary

Technical Problem

Conventional polyamide, polyethylene terephthalate, and polypropylene resins used in packaging materials face issues such as high heat-sealing temperatures, film shrinkage during heat-sealing, poor packaging appearance, and low heat-sealing strength, limiting packaging speed and processability, while existing ethylene ionomers with multi-branched molecular structures lack sufficient strength and hot tack properties.

Method used

A novel ethylene-based ionomer with a substantially linear molecular structure, produced using a late transition metal catalyst, is integrated into a resin composition that includes structural units derived from ethylene, α-olefins, and monomers with carboxyl or dicarboxylic acid anhydride groups, converted into metal-containing carboxylates, enhancing heat-sealing properties, particularly hot tack strength.

Benefits of technology

The resin composition achieves improved heat-sealing properties and hot tack strength, allowing for faster packaging processes and reduced sealant layer thickness, thereby improving packaging material performance and cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567225000023
    Figure 0007567225000023
  • Figure 0007567225000024
    Figure 0007567225000024
  • Figure 0007567225000025
    Figure 0007567225000025
Patent Text Reader

Abstract

To provide a polymer resin composition for lamination using an ionomer which is excellent in workability and hot tack strength, and a laminate.SOLUTION: A composition contains (X1) 100-60 wt.% of an ionomer in which at least a part of a carboxyl group and / or a dicarboxylic acid anhydride group in a copolymer (P) containing a structural unit (A) derived from ethylene and / or α-olefin having 3-20 carbon atoms and a structural unit (B) derived from a monomer having a carboxyl group and / or a dicarboxylic acid anhydride group as essential structural units is converted into a metal-containing carboxylate containing at least one metal ion selected from Group I, II or XII in the periodic table, and a phase angle δ at an absolute value G*=0.1 MPa of complex modulus of elasticity measured by a rotary type rheometer is 50-75 degrees; and (X2) 40-0 wt.% of an ethylenic copolymer containing ethylene by high pressure radial polymerization as an essential monomer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polymer composition for lamination using a novel ionomer and a laminate using the same. [Background technology]

[0002] Conventionally, polyamide resins, polyethylene terephthalate resins, polypropylene resins, etc., which are excellent in transparency and mechanical strength, have been used as packaging substrates. However, these resins have problems such as high heat sealing temperatures, which make it impossible to increase the packaging speed, deterioration of the packaging appearance due to shrinkage of the film during heat sealing, and low heat sealing strength. For this reason, these substrates are rarely used alone, and usually, composite films are used in which these substrates are used as substrates for lamination and a heat seal layer obtained by laminating a polyethylene resin or the like thereon is provided. For example, composite films in which a sealant layer is provided on a surface substrate layer, or packaging films obtained by laminating various intermediate layers on a substrate and further laminating a sealant layer thereon, are known as substrates for liquid packaging.

[0003] On the other hand, ethylene-based ionomers are resins that use ethylene-unsaturated carboxylic acid copolymers as a base resin and are intermolecularly bonded with metal ions such as sodium and zinc (Patent Document 1). They are strong, elastic, flexible, abrasion-resistant, and transparent. Currently, commercially available ethylene-based ionomers include "Surlyn (registered trademark)", a sodium salt or zinc salt of ethylene-methacrylic acid copolymer developed by Dupont, and "Himilan (registered trademark)" sold by Dow Mitsui Polychemicals.

[0004] The ethylene-unsaturated carboxylic acid copolymers used as the base resins for these currently commercially available ethylene-based ionomers all use polar group-containing olefin copolymers obtained by polymerizing ethylene and polar group-containing monomers such as unsaturated carboxylic acids by high-pressure radical polymerization. The high-pressure radical polymerization method has the advantage that it is possible to polymerize relatively any type of polar group-containing monomer at low cost. However, the molecular structure of the polar group-containing olefin copolymer produced by the high-pressure radical polymerization method is a multi-branched molecular structure having many irregular long-chain branches and short-chain branches, as shown in the image diagram in Figure 1, and has the disadvantage of being insufficient in terms of strength.

[0005] Meanwhile, methods have been explored for producing polar group-containing olefin copolymers with a linear molecular structure, as shown in the image in Figure 2, using a polymerization method that uses a catalyst. However, polar group-containing monomers are generally catalyst poisons, making polymerization difficult. In fact, it has been considered difficult for many years to obtain polar group-containing olefin copolymers with the desired physical properties using an industrially inexpensive and stable method. However, in recent years, the applicants of the present application have proposed a method for industrially and inexpensively obtaining polar group-containing olefin copolymers having a substantially linear molecular structure in a stable manner by using a new catalyst and a new production method. The applicants of the present application have reported that they have succeeded in producing a copolymer of ethylene and t-butyl acrylate using a late transition metal catalyst as a method for producing a polar group-containing olefin copolymer that serves as the base resin for an ethylene-based ionomer, and modifying the resulting polar group-containing olefin copolymer by heat or acid treatment to form an ethylene-acrylic acid copolymer, which is then reacted with metal ions to produce a binary ionomer (Patent Document 2). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] U.S. Pat. No. 3,264,272 [Patent Document 2] JP 2016-79408 A Summary of the Invention [Problem to be solved by the invention]

[0007] Low density polyethylene (LDPE) and ethylene-vinyl acetate copolymer (EVA) were initially used as laminating polymers for forming the sealant layer of composite films. However, LDPE films have problems with low-temperature heat sealability, heat resistance, and hot tack properties, while EVA has problems with heat resistance and hot tack properties. In addition, conventionally known ethylene ionomers with a multi-branched molecular structure are not strong enough, and the inventors have found that they also have problems with heat sealability, especially hot tack strength. Low hot tack strength affects packaging speed and processability, for example by making it impossible to fill the contents in the molten state immediately after sealing. In view of the above-mentioned state of the art, the present application has an object to provide a polymer resin composition for lamination using an ionomer that has excellent processability and hot tack strength, and a laminate. [Means for solving the problem]

[0008] The ethylene-based ionomer described in Patent Document 2 is a novel ethylene-based ionomer that has not been seen before, in which the base resin has a substantially linear molecular structure and also functions as an ionomer. Its physical properties, etc. are significantly different from those of conventional ethylene-based ionomers, and its unique characteristics and suitable applications were also unknown. As a result of intensive research conducted by the present inventors in order to solve the above-mentioned problems, it was found that by using a resin composition containing an ethylene-based ionomer in which an ester group of an ethylene / unsaturated carboxylate copolymer obtained from ethylene and an unsaturated carboxylate using a late transition metal catalyst is converted into a metal-containing carboxylate, a polymer resin composition for lamination having excellent processability can be obtained, and by using this polymer resin composition for lamination in a sealant layer of a laminate, a laminate having better heat seal properties, particularly better hot tack properties, can be obtained than ionomers based on polar group-containing olefin copolymers obtained by conventional high-pressure radical polymerization methods, which led to the completion of the present invention.

[0009] That is, the present invention is as described in the following [1] to

[13] . [1] (X1) A copolymer (P) containing, as essential constituent units, structural units (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms and structural units (B) derived from a monomer having a carboxyl group and / or a dicarboxylic anhydride group, in which at least a portion of the carboxyl groups and / or dicarboxylic anhydride groups are converted into a metal-containing carboxylate containing at least one metal ion selected from Groups 1, 2, or 12 of the periodic table, and the absolute value G of the complex modulus measured with a rotational rheometer is * 100 to 60% by weight of an ionomer having a phase angle δ of 50 degrees to 75 degrees at σ = 0.1 MPa; (X2) Ethylene-based copolymer with ethylene as the essential monomer by high pressure radical polymerization 40-0% by weight and has a melt flow rate of 1.0 to 100 g / 10 min. [2] (X1) A copolymer (P) containing, as essential structural units, a structural unit (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms and a structural unit (B) derived from a monomer having a carboxyl group and / or a dicarboxylic anhydride group, and further containing, as a structural unit, a structural unit (C) other than the structural unit (A) and the structural unit (B) which is a compound having one or more carbon-carbon double bonds in its molecular structure, at least a part of the carboxyl groups and / or dicarboxylic anhydride groups in the copolymer (P) is converted to a metal-containing carboxylate containing at least one metal ion selected from Groups 1, 2, or 12 of the periodic table, and the absolute value G of the complex modulus measured with a rotational rheometer is * 100 to 60% by weight of an ionomer having a phase angle δ of 50 degrees to 75 degrees at σ = 0.1 MPa; (X2) Ethylene-based copolymer with ethylene as the essential monomer by high pressure radical polymerization 40-0% by weight and has a melt flow rate of 1.0 to 100 g / 10 min. [3] The polymer composition for lamination according to [2], wherein the structural unit (C) in the copolymer (P) is a non-cyclic monomer represented by the following general formula (1) or a cyclic monomer represented by the following general formula (2): [ka] [In general formula (1), T 1 ~T 3 each independently represents a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a hydroxyl group, a hydrocarbon group having 2 to 20 carbon atoms substituted with an alkoxy group having 1 to 20 carbon atoms, a hydrocarbon group having 3 to 20 carbon atoms substituted with an ester group having 2 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an ester group having 2 to 20 carbon atoms, a silyl group having 3 to 20 carbon atoms, a halogen atom, or a cyano group; T 4is a substituent selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms substituted with a hydroxyl group, a hydrocarbon group having 2 to 20 carbon atoms substituted with an alkoxy group having 1 to 20 carbon atoms, a hydrocarbon group having 3 to 20 carbon atoms substituted with an ester group having 2 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an ester group having 2 to 20 carbon atoms, a silyl group having 3 to 20 carbon atoms, a halogen atom, or a cyano group. [ka] [In general formula (2), R 1 ~R 12 may be the same or different and are selected from the group consisting of a hydrogen atom, a halogen atom, and a hydrocarbon group having 1 to 20 carbon atoms; R 9 and R 10 , and R 11 and R 12 may combine together to form a divalent organic group, R 9 or R 10 And, R 11 or R 12 may form a ring together. In addition, n represents 0 or a positive integer, and when n is 2 or more, R 5 ~R 8 may be the same or different in each repeating unit. [4] The polymer composition for lamination according to [3], wherein the structural unit (C) in the copolymer (P) is a non-cyclic monomer represented by the general formula (1). [5] The polymer composition for lamination according to [3], wherein the structural unit (C) in the copolymer (P) is a cyclic monomer represented by the general formula (2). [6] The copolymer (P) 13 The polymer composition for lamination according to any one of [1] to [5], characterized in that the number of methyl branches calculated by C-NMR is 50 or less per 1,000 carbons. [7] The copolymer (P)13 The polymer composition for lamination according to any one of [1] to [5], characterized in that the number of methyl branches calculated by C-NMR is 5 or less per 1,000 carbons. [8] The polymer composition for lamination according to any one of [1] to [7], wherein the copolymer (P) contains the structural unit (B) in an amount of 2 to 20 mol % in the copolymer. [9] The polymer composition for lamination according to any one of [1] to [8], wherein the structural unit (A) is a structural unit derived from ethylene.

[10] The polymer composition for lamination according to any one of [1] to [9], wherein the copolymer (P) is produced using a transition metal catalyst containing a transition metal of Groups 8 to 11 of the periodic table.

[11] The polymer composition for lamination according to

[10] , wherein the transition metal catalyst is a transition metal catalyst comprising a phosphorus sulfonic acid or phosphorus phenol ligand and nickel or palladium.

[12] The polymer composition for lamination according to any one of [1] to

[11] , wherein the ethylene copolymer obtained by high-pressure radical polymerization (X2) is an ethylene homopolymer.

[13] A laminate comprising at least a layer I consisting of a base material layer and a layer II consisting of a sealant layer, wherein the sealant layer is made of the polymer composition for lamination according to any one of [1] to

[12] . Effect of the Invention

[0010] The polymer resin composition for lamination using the ionomer of the present invention, which has a substantially linear structure, has significantly better heat seal properties, especially hot tack properties, than ionomers based on polar group-containing olefin copolymers obtained by conventional high-pressure radical polymerization methods. When this resin composition is used as a sealant layer, a laminate having excellent heat seal properties, especially good hot tack properties, can be obtained. This not only enables the cycle time to be increased in the heat sealing process, but also enables the gauge-down of the sealant layer to reduce the volume and costs, thereby improving the performance as a packaging material. [Brief description of the drawings]

[0011] [Figure 1] 1 is a conceptual diagram of the molecular structure of a multi-branched polar group-containing olefin copolymer produced by high-pressure radical polymerization. The circles in the diagram represent polar groups. [Diagram 2] 1 is a conceptual diagram of a linear olefin copolymer containing a polar group, in which the circles represent polar groups. [Diagram 3] 1 is a graph showing hot tack strength versus temperature in Examples 1 and 2 and Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present invention relates to (X1) 100 to 60% by weight of an ionomer comprising a copolymer (P) as a base resin, the copolymer (P) comprising, as essential constituent units, structural units (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms, and structural units (B) derived from a monomer having a carboxyl group and / or a dicarboxylic anhydride group, and optionally a structural unit (C) which is a compound having one or more carbon-carbon double bonds in the molecular structure, and which is copolymerized, preferably randomly, in a substantially linear manner, and at least a portion of the carboxyl groups and / or dicarboxylic anhydride groups of the structural unit (B) is converted to a metal-containing carboxylate containing at least one metal ion selected from Groups 1, 2, and 12 of the periodic table; (X2) Ethylene-based copolymer with ethylene as the essential monomer by high pressure radical polymerization 40-0% by weight The polymer composition for lamination is a resin composition consisting of the above-mentioned, and is characterized in that the melt flow rate of the composition is 1.0 to 100 g / 10 min.; and a laminate using the same.

[0013] The ionomer according to the present invention, the polymer resin composition for lamination using the ionomer, the laminate using the same, and the uses thereof will be described in detail below. In this specification, "(meth)acrylic acid" means acrylic acid or methacrylic acid. In this specification, "to" indicating a numerical range is used to mean that the numerical values ​​before and after it are included as the lower and upper limits. In this specification, a copolymer means a binary or higher copolymer containing at least one type of unit (A) and at least one type of unit (B). In addition, in this specification, the ionomer refers to an ionomer of a binary or higher copolymer that contains the structural unit (A) and a structural unit (B') in which at least a portion of the structural unit (B) is converted to a metal-containing carboxylate, and may further contain the structural unit (B).

[0014] 1. Ionomer The ionomer, which is the component (X1) of the present invention, is characterized in that it contains, as essential constituent units, structural units (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms, and structural units (B) derived from a monomer having a carboxyl group and / or a dicarboxylic anhydride group, and optionally also contains, as a constituent unit, a structural unit (C) which is a compound having one or more carbon-carbon double bonds in its molecular structure, and uses as a base resin a copolymer (P) in which these are copolymerized, preferably randomly copolymerized, in a substantially linear manner, and that at least a portion of the carboxyl groups and / or dicarboxylic anhydride groups of the structural unit (B) are converted to a metal-containing carboxylate containing at least one metal ion selected from Group 1, Group 2, or Group 12 of the periodic table.

[0015] (1) Structural unit (A) The structural unit (A) is at least one structural unit selected from the group consisting of structural units derived from ethylene and structural units derived from an α-olefin having 3 to 20 carbon atoms. The α-olefins involved in the present invention have the structural formula: CH2=CHR 18 is an α-olefin having 3 to 20 carbon atoms (R 18 is a hydrocarbon group having 1 to 18 carbon atoms, which may have a linear structure or may be branched.) The α-olefin more preferably has 3 to 12 carbon atoms.

[0016] Specific examples of the structural unit (A) include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, 3-methyl-1-butene, and 4-methyl-1-pentene, and may be ethylene. As the ethylene, ethylene derived from a petroleum raw material or a non-petroleum raw material such as a plant raw material can be used. The structural unit (A) may be of one type or of multiple types. Examples of combinations of the two include ethylene-propylene, ethylene-1-butene, ethylene-1-hexene, ethylene-1-octene, propylene-1-butene, propylene-1-hexene, and propylene-1-octene. Examples of combinations of the three include ethylene-propylene-1-butene, ethylene-propylene-1-hexene, ethylene-propylene-1-octene, propylene-1-butene-hexene, and propylene-1-butene-1-octene.

[0017] In the present invention, the structural unit (A) preferably contains ethylene as an essential component and may further contain one or more α-olefins having 3 to 20 carbon atoms, if necessary. The amount of ethylene in the structural unit (A) may be 65 to 100 mol % or 70 to 100 mol % based on the total moles of the structural unit (A). In terms of impact resistance, the structural unit (A) may be a structural unit derived from ethylene.

[0018] (2) Structural unit (B) The structural unit (B) is a structural unit derived from a monomer having a carboxyl group and / or a dicarboxylic anhydride group. Note that the structural unit (B) has the same structure as the structural unit derived from a monomer having a carboxyl group and / or a dicarboxylic anhydride group, and as described later in the production method, it does not necessarily have to be produced using a monomer having a carboxyl group and / or a dicarboxylic anhydride group.

[0019] Examples of structural units derived from monomers having a carboxyl group include unsaturated carboxylic acids such as acrylic acid, methacrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, norbornene dicarboxylic acid, and bicyclo[2,2,1]hept-2-ene-5,6-dicarboxylic acid. Examples of structural units derived from monomers having a dicarboxylic acid anhydride group include maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, 5-norbornene-2,3-dicarboxylic anhydride, 3,6-epoxy-1,2,3,6-tetrahydrophthalic anhydride, and tetracyclo[6.2.1.1 3,6 .0 2,7 ] Unsaturated dicarboxylic acid anhydrides such as dodec-9-ene-4,5-dicarboxylic acid anhydride and 2,7-octadien-1-yl succinic acid anhydride are exemplified. As the structural unit derived from a monomer having a carboxyl group and / or a dicarboxylic anhydride group, from the viewpoint of industrial availability, preferred examples include structural units derived from acrylic acid, methacrylic acid, and 5-norbornene-2,3-dicarboxylic anhydride, and in particular, structural units derived from acrylic acid. Furthermore, the structural unit derived from a monomer having a carboxyl group and / or a dicarboxylic anhydride group may be of one type or of multiple types.

[0020] In addition, the dicarboxylic anhydride group may react with moisture in the air to open the ring and become a part of the dicarboxylic acid, but the dicarboxylic anhydride group may be in a ring-opened state as long as it does not deviate from the gist of the present invention.

[0021] (3) Other structural units (C) The copolymer (P) according to the present invention may be a binary copolymer consisting of only the structural unit (A) and the structural unit (B), or a multicomponent copolymer containing the structural unit (A), the structural unit (B), and a structural unit (C) other than the structural units (A) and (B). The multicomponent copolymer is preferably a multicomponent copolymer containing a structural unit (C) other than the structural units represented by the structural units (A) and (B). The monomer that gives the structural unit (C) may be any monomer as long as it is not included in the monomers that give the structural unit (A) and the structural unit (B). The monomer that gives the structural unit (C) is not limited as long as it is a compound having one or more carbon-carbon double bonds in the molecular structure, and may be, for example, an acyclic monomer represented by the general formula (1) or a cyclic monomer represented by the general formula (2). Compared with a binary copolymer consisting of only the structural unit (A) and the structural unit (B), by using a ternary or higher multi-component copolymer containing the structural unit (C) as the base resin of the ionomer, a polymer for lamination that is more flexible than a binary copolymer can be obtained when used for lamination, and a polymer composition for lamination that is also superior in heat seal properties and hot tack properties can be obtained. The structural unit (C) may be based on one type of monomer, or may be a combination of two or more types of monomers.

[0022] Acyclic Monomers [ka] [In general formula (1), T 1 ~T 3each independently represents a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a hydroxyl group, a hydrocarbon group having 2 to 20 carbon atoms substituted with an alkoxy group having 1 to 20 carbon atoms, a hydrocarbon group having 3 to 20 carbon atoms substituted with an ester group having 2 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an ester group having 2 to 20 carbon atoms, a silyl group having 3 to 20 carbon atoms, a halogen atom, or a cyano group; T 4 is a substituent selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms substituted with a hydroxyl group, a hydrocarbon group having 2 to 20 carbon atoms substituted with an alkoxy group having 1 to 20 carbon atoms, a hydrocarbon group having 3 to 20 carbon atoms substituted with an ester group having 2 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an ester group having 2 to 20 carbon atoms, a silyl group having 3 to 20 carbon atoms, a halogen atom, or a cyano group.

[0023] T 1 ~T 4 The carbon skeleton of the hydrocarbon group, substituted alkoxy group, substituted ester group, alkoxy group, aryl group, ester group and silyl group may have a branch, a ring, and / or an unsaturated bond. T 1 ~T 4 The lower limit of the number of carbon atoms in the hydrocarbon group may be 1 or more, and the upper limit may be 20 or less, or may be 10 or less. T 1 ~T 4 The lower limit of the number of carbon atoms in the substituted alkoxy group may be 1 or more, and the upper limit may be 20 or less, or may be 10 or less. T 1 ~T 4 The lower limit of the number of carbon atoms in the substituted ester group may be 2 or more, and the upper limit may be 20 or less, or may be 10 or less. T 1 ~T 4The lower limit of the number of carbon atoms in the alkoxy group may be 1 or more, and the upper limit may be 20 or less, or may be 10 or less. T 1 ~T 4 The lower limit of the number of carbon atoms in the aryl group in the above formula may be 6 or more, and the upper limit may be 20 or less, or may be 11 or less. T 1 ~T 4 The lower limit of the number of carbon atoms in the ester group may be 2 or more, and the upper limit may be 20 or less, or may be 10 or less. T 1 ~T 4 The number of carbon atoms in the silyl group in the above formula may be 3 or more, and may be 18 or less, or may be 12 or less. Examples of the silyl group include a trimethylsilyl group, a triethylsilyl group, a tri-n-propylsilyl group, a triisopropylsilyl group, a dimethylphenylsilyl group, a methyldiphenylsilyl group, and a triphenylsilyl group.

[0024] In the ionomer of the present invention, from the viewpoint of ease of production, T 1 and T 2 may be a hydrogen atom, T 3 may be a hydrogen atom or a methyl group, T 1 ~T 3 However, each of them may be a hydrogen atom. In terms of impact resistance, T 4 may be an ester group having 2 to 20 carbon atoms.

[0025] Specific examples of the non-cyclic monomer include T 4 is an ester group having 2 to 20 carbon atoms. T 4 is an ester group having 2 to 20 carbon atoms, the acyclic monomer may be a monomer having the structural formula: CH2=C(R 21 )CO2(R 22 ) where R 21 R is a hydrogen atom or a hydrocarbon group having 1 to 10 carbon atoms, which may have a branch, a ring, and / or an unsaturated bond.22 is a hydrocarbon group having 1 to 20 carbon atoms, which may have a branch, a ring, and / or an unsaturated bond. 22 It may contain a heteroatom at any position within the group. Structural formula: CH2=C(R 21 )CO2(R 22 ) as a compound represented by R 21 is a hydrogen atom or a hydrocarbon group having 1 to 5 carbon atoms. 21 is a hydrogen atom, or R 21 Methacrylate esters in which the alkyl group is a methyl group are also included. Structural formula: CH2=C(R 21 )CO2(R 22 Specific examples of the compound represented by the formula (1) include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, octadecyl (meth)acrylate, phenyl (meth)acrylate, toluyl (meth)acrylate, and benzyl (meth)acrylate. Specific compounds include methyl acrylate, ethyl acrylate, n-butyl acrylate (nBA), isobutyl acrylate (iBA), t-butyl acrylate (tBA), and 2-ethylhexyl acrylate, and may in particular be n-butyl acrylate (nBA), isobutyl acrylate (iBA), and t-butyl acrylate (tBA). The non-cyclic monomer may be of one type or of multiple types.

[0026] Cyclic Monomers [ka] [In general formula (2), R 1 ~R 12 may be the same or different and are selected from the group consisting of a hydrogen atom, a halogen atom, and a hydrocarbon group having 1 to 20 carbon atoms; R 9 and R 10 , and R 11 and R 12 may combine together to form a divalent organic group, R 9 or R 10 And, R 11 or R 12 may form a ring together. In addition, n represents 0 or a positive integer, and when n is 2 or more, R 5 ~R 8 may be the same or different in each repeating unit.

[0027] Examples of the cyclic monomer include norbornene-based olefins, such as norbornene, vinylnorbornene, ethylidenenorbornene, norbornadiene, tetracyclododecene, tricyclo[4.3.0.1 2,5 ], Tricyclo[4.3.0.1 2,5 ]dec-3-ene, and other compounds having a cyclic olefin skeleton. 3,6 .0 2,7 ]dodec-4-ene and the like.

[0028] (4) Copolymer (P) The copolymer (P) used in the present invention as the base resin of the ionomer contains, as essential constituent units, a structural unit (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms, and a structural unit (B) derived from a monomer having a carboxyl group and / or a dicarboxylic anhydride group, and may further contain an arbitrary structural unit (C) other than the above (A) and (B), which are copolymerized substantially linearly, preferably randomly. Here, "substantially linear" refers to a state in which the copolymer has no branch or the frequency of branched structures is low, and the copolymer can be considered to be linear. Specifically, it refers to a state in which the phase angle δ of the copolymer is 50 degrees or more under the conditions described below.

[0029] The copolymer according to the present invention must contain at least one type of structural unit (A) and at least one type of structural unit (B), for a total of two or more types of monomer units. It may also contain any structural unit (C) other than (A) and (B), but is preferably a multicomponent copolymer containing such a structural unit (C). The structural units and the amounts of the structural units in the copolymer according to the present invention will be described below. A structure derived from one molecule each of ethylene and / or an α-olefin having 3 to 20 carbon atoms (A), a monomer having a carboxyl group and / or a dicarboxylic anhydride group (B), and any monomer (C) other than (A) and (B) is defined as one structural unit in the copolymer. The amount of structural units is the ratio of each structural unit expressed in mol % when all structural units in the copolymer are taken as 100 mol %.

[0030] Amount of structural units of ethylene and / or α-olefin having 3 to 20 carbon atoms (A): The structural unit amount of the structural unit (A) according to the present invention is selected from the following: lower limit is 60.0 mol% or more, preferably 70.0 mol% or more, more preferably 80.0 mol% or more, even more preferably 85.0 mol% or more, still more preferably 90.0 mol% or more, and particularly preferably 91.2 mol% or more, and upper limit is 97.9 mol% or less, preferably 97.5 mol% or less, more preferably 97.0 mol% or less, and even more preferably 96.5 mol% or less. If the amount of structural units derived from ethylene and / or an α-olefin (A) having 3 to 20 carbon atoms is less than 60.0 mol%, the toughness of the copolymer will be inferior, and if it is more than 97.9 mol%, the crystallinity of the copolymer will be high, and the transparency may be deteriorated.

[0031] Amount of structural units of monomer (B) having a carboxyl group and / or a dicarboxylic anhydride group: The amount of the structural unit (B) according to the present invention is selected from the following: the lower limit is 2.0 mol% or more, preferably 2.9 mol% or more, and more preferably 5.2 mol% or more, and the upper limit is 20.0 mol% or less, preferably 15.0 mol% or less, more preferably 10.0 mol% or less, even more preferably 8.0 mol% or less, particularly preferably 6.0 mol% or less, and most preferably 5.6 mol% or less. If the amount of structural units derived from monomer (B) having a carboxyl group and / or a dicarboxylic anhydride group is less than 2.0 mol%, the copolymer may not have sufficient adhesion to highly polar dissimilar materials, and if it exceeds 20.0 mol%, the copolymer may not have sufficient mechanical properties. Furthermore, the monomer having a carboxyl group and / or a dicarboxylic anhydride group to be used may be used alone or in combination of two or more kinds.

[0032] Amount of structural units of any monomer (C): When the components of the ionomer of the present invention contain any monomer other than the (A) and (B), the structural unit amount of the structural unit (C) is selected from the following: the lower limit is 0.001 mol% or more, preferably 0.010 mol% or more, more preferably 0.020 mol% or more, even more preferably 0.1 mol% or more, still more preferably 1.9 mol% or more, and particularly preferably 2.0 mol% or more, and the upper limit is 20.0 mol% or less, preferably 15.0 mol% or less, more preferably 10.0 mol% or less, even more preferably 5.0 mol% or less, and particularly preferably 3.6 mol% or less. When the amount of the structural unit derived from any monomer (C) is 0.001 mol % or more, the flexibility of the copolymer tends to be sufficient, and when it is 20.0 mol % or less, the mechanical properties of the copolymer tend to be sufficient. Any of the monomers used may be used alone or in combination of two or more kinds.

[0033] Number of branches per 1,000 carbons in copolymer: In the copolymer of the present invention, in order to increase the elastic modulus and obtain sufficient mechanical properties, 13 The number of methyl branches calculated by C-NMR may be 50 or less, 5.0 or less, 1.0 or less, or 0.5 or less per 1,000 carbons, with no particular limit on the lower limit, and the smaller the better. The number of ethyl branches may be 3.0 or less, 2.0 or less, 1.0 or less, or 0.5 or less per 1,000 carbons, with no particular limit on the lower limit, and the smaller the better. The number of butyl branches may be 7.0 or less, 5.0 or less, 3.0 or less, or 0.5 or less per 1,000 carbons, with no particular limit on the lower limit, and the smaller the better.

[0034] Method for measuring the amount of structural units derived from monomers having a carboxy group and / or a dicarboxylic anhydride group and non-cyclic monomers in a copolymer, and the number of branches: The amount of structural units derived from monomers having a carboxy group and / or a dicarboxylic anhydride group and non-cyclic monomers in the copolymer of the present invention, and the number of branches per 1,000 carbon atoms are 13 It can be determined using C-NMR spectroscopy. 13 C-NMR is measured by the following method. 200-300 mg of sample is placed in an NMR sample tube with an inner diameter of 10 mm together with 2.4 ml of a mixed solvent of o-dichlorobenzene (C6H4Cl2) and deuterated bromide benzene (C6D5Br) (C6H4Cl2 / C6D5Br = 2 / 1 (volume ratio)) and hexamethyldisiloxane, a chemical shift standard substance, and the tube is sealed after replacing with nitrogen. It is heated and dissolved to prepare a homogeneous solution, which is used as the NMR measurement sample. NMR measurements are performed at 120°C using an AV400M NMR instrument from Bruker Japan Ltd. equipped with a 10 mmφ cryoprobe. 13 C-NMR was measured using the inverse gate decoupling method with a sample temperature of 120°C, a pulse angle of 90°, a pulse interval of 51.5 seconds, and an accumulation count of 512 or more. The chemical shifts are those of hexamethyldisiloxane. 13 The C signal was set at 1.98 ppm, and the other 13 The chemical shifts of the C signals are based on this. Obtained 13 In C-NMR, the amount of structural units of each monomer in the copolymer and the number of branches can be analyzed by identifying signals specific to the monomers or branches contained in the copolymer and comparing their intensities. The positions of signals specific to the monomers or branches can be referred to publicly known materials or can be independently identified depending on the sample. Such analytical techniques are commonly known to those skilled in the art.

[0035] Weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn): The weight average molecular weight (Mw) of the copolymer according to the present invention has a lower limit of usually 1,000 or more, preferably 6,000 or more, and more preferably 10,000 or more, and an upper limit of usually 2,000,000 or less, preferably 1,500,000 or less, even more preferably 1,000,000 or less, particularly preferably 800,000 or less, and most preferably 100,000 or less. If the Mw is less than 1,000, the physical properties such as mechanical strength and impact resistance of the copolymer will be insufficient, whereas if the Mw exceeds 2,000,000, the melt viscosity of the copolymer will be extremely high, making it difficult to mold the copolymer.

[0036] The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the copolymer according to the present invention is usually in the range of 1.5 to 4.0, preferably 1.6 to 3.5, and more preferably 1.9 to 2.3. If Mw / Mn is less than 1.5, the copolymer may have insufficient processability, including molding, whereas if it exceeds 4.0, the copolymer may have poor mechanical properties. In the present invention, (Mw / Mn) may be expressed as a molecular weight distribution parameter.

[0037] The weight average molecular weight (Mw) and number average molecular weight (Mn) of the copolymer according to the present invention are determined by gel permeation chromatography (GPC). The molecular weight distribution parameter (Mw / Mn) is calculated by determining the number average molecular weight (Mn) by gel permeation chromatography (GPC) and then calculating the ratio of Mw to Mn, Mw / Mn.

[0038] An example of the GPC measurement method according to the present invention is as follows. (Measurement conditions) Machine used: Waters 150C Detector: FOXBORO MIRAN1A IR detector (measurement wavelength: 3.42 μm) Measurement temperature: 140℃ Solvent: orthodichlorobenzene (ODCB) Column: Showa Denko AD806M / S (3 columns) Flow rate: 1.0mL / min Injection volume: 0.2mL (Sample preparation) A 1 mg / mL solution of the sample is prepared using ODCB (containing 0.5 mg / mL BHT (2,6-di-t-butyl-4-methylphenol)), and dissolved at 140° C. for about 1 hour. (Calculation of molecular weight (M)) The standard polystyrene method is used, and the conversion from retention volume to molecular weight is performed using a calibration curve of standard polystyrene that has been prepared in advance. The standard polystyrene used is, for example, Tosoh's (F380, F288, F128, F80, F40, F20, F10, F4, F1, A5000, A2500, A1000) brand, Showa Denko's monodisperse polystyrene (S-7300, S-3900, S-1950, S-1460, S-1010, S-565, S-152, S-66.0, S-28.5, S-5.05, each 0.07 mg / ml solution), etc. A calibration curve is prepared by injecting 0.2 mL of a solution in which each is dissolved in ODCB (containing 0.5 mg / mL BHT) so that the concentration is 0.5 mg / mL. The calibration curve is a cubic equation obtained by approximating the least squares method, or a quartic equation obtained by approximating the logarithm of the elution time and molecular weight. The viscosity equation used to convert to molecular weight (M) is [η] = K × Mα, and the following values ​​are used. Polystyrene (PS): K = 1.38 x 10 -4 , α=0.7 Polyethylene (PE): K = 3.92 x 10 -4 , α=0.733 Polypropylene (PP): K = 1.03 x 10 -4 , α=0.78

[0039] Melting point (Tm, ℃): The melting point of the copolymer according to the present invention is indicated by the maximum peak temperature of the endothermic curve measured by a differential scanning calorimeter (DSC). When multiple peaks are shown in the endothermic curve obtained by DSC measurement, with heat flow (mW) on the vertical axis and temperature (°C) on the horizontal axis, the maximum peak temperature refers to the temperature of the peak with the maximum height from the baseline among the multiple peaks, or when there is only one peak, the maximum peak temperature refers to the temperature of that peak. The melting point is preferably 50° C. to 140° C., more preferably 60° C. to 138° C., and most preferably 70° C. to 135° C. If it is lower than this range, the heat resistance is insufficient, and if it is higher than this range, the adhesiveness may be poor. In the present invention, the melting point can be determined from the absorption curve obtained by, for example, using a DSC (DSC7020) manufactured by SII Nano Technology Inc., packing about 5.0 mg of a sample into an aluminum pan, heating it to 200°C at 10°C / min, holding it isothermally at 200°C for 5 minutes, lowering it to 20°C at 10°C / min, holding it isothermally at 20°C for 5 minutes, and then heating it again to 200°C at 10°C / min.

[0040] Crystallinity (%): In the copolymer of the present invention, the crystallinity observed by differential scanning calorimetry (DSC) is not particularly limited, but is preferably more than 0% and not more than 30%, more preferably more than 0% and not more than 25%, particularly preferably more than 5% and not more than 25%, and most preferably 7% or more and not more than 24%. In the present invention, the crystallinity can be determined, for example, by determining the heat of fusion (ΔH) from the area of ​​the melting endothermic peak obtained by DSC measurement using the same procedure as in the measurement of the melting point, and dividing the heat of fusion by the heat of fusion of 293 J / g of perfect crystals of high density polyethylene (HDPE).

[0041] Molecular structure of copolymer: The molecular chain terminals of the copolymer according to the present invention may be structural units (A) of ethylene and / or an α-olefin having 3 to 20 carbon atoms, structural units (B) of a monomer having a carboxyl group and / or a dicarboxylic anhydride group, or structural units (C) of any monomer other than (A) and (B).

[0042] The copolymer according to the present invention may be a random copolymer, block copolymer, graft copolymer, etc., of a structural unit (A) of ethylene and / or an α-olefin having 3 to 20 carbon atoms, a structural unit (B) of a monomer having a carboxyl group and / or a dicarboxylic anhydride group, and a structural unit (C) of an arbitrary monomer. Among these, a random copolymer that can contain a large amount of the structural unit (B) may be used. An example of the molecular structure of a typical ternary copolymer (1) is shown below. A random copolymer is a copolymer in which the probability of finding a structural unit (A) of ethylene and / or an α-olefin having 3 to 20 carbon atoms, a structural unit (B) of a monomer having a carboxyl group and / or a dicarboxylic anhydride group, and a structural unit (C) of an arbitrary monomer at a position in an arbitrary molecular chain, as shown in the molecular structure example (1) below, is independent of the type of the adjacent structural unit. As shown below, in the molecular structure example (1) of the copolymer, a structural unit (A) of ethylene and / or an α-olefin having 3 to 20 carbon atoms, a structural unit (B) of a monomer having a carboxyl group and / or a dicarboxylic anhydride group, and a structural unit (C) of an arbitrary monomer form a random copolymer. [ka]

[0043] For reference, an example of a molecular structure (2) of a copolymer into which structural unit (B) of a monomer having a carboxyl group and / or a dicarboxylic anhydride group has been introduced by graft modification is shown. A part of a copolymer in which structural unit (A) of ethylene and / or an α-olefin having 3 to 20 carbon atoms and structural unit (C) of an arbitrary monomer are copolymerized is graft modified with structural unit (B) of a monomer having a carboxyl group and / or a dicarboxylic anhydride group. [ka]

[0044] In addition, the random copolymerization of a copolymer can be confirmed by various methods, but a method for determining the random copolymerization from the relationship between the comonomer content and melting point of the copolymer is described in detail in JP 2015-163691 A and JP 2016-079408 A. From the above documents, it can be determined that the randomness is low when the melting point (Tm, °C) of the copolymer is higher than -3.74 × [Z] + 130 (where [Z] is the comonomer content / mol%).

[0045] The copolymer according to the present invention preferably has a melting point (Tm, °C) measured by differential scanning calorimetry (DSC) and a total content [Z] (mol %) of the structural unit (B) of the monomer having a carboxyl group and / or a dicarboxylic anhydride group and the structural unit (C) of an arbitrary monomer, which satisfy the following formula (I): 50 <Tm<-3.74×[Z]+130···(I) If the melting point of the copolymer (Tm, °C) is higher than -3.74 × [Z] + 130 (°C), the random copolymerization is low, resulting in poor mechanical properties such as impact strength. If the melting point is lower than 50°C, the heat resistance may be poor.

[0046] Furthermore, the copolymer according to the present invention is preferably produced in the presence of a transition metal catalyst, from the viewpoint of making the molecular structure thereof linear. It is known that the molecular structure of the copolymer varies depending on the production method, such as polymerization by a high-pressure radical polymerization process or polymerization using a metal catalyst. The difference in molecular structure can be controlled by selecting the production method, but the molecular structure can also be estimated from the complex modulus measured with a rotational rheometer, as described in JP 2010-150532 A, for example.

[0047] · Absolute value of complex elastic modulus G * Phase angle δ at =0.1MPa: In the copolymer of the present invention, the absolute value of the complex modulus G measured by a rotational rheometer * The phase angle δ at σ = 0.1 MPa may have a lower limit of 50 degrees or more, 51 degrees or more, 54 degrees or more, 56 degrees or more, or 58 degrees or more, and an upper limit of 75 degrees or less, or 70 degrees or less. More specifically, the absolute value of the complex modulus G measured by a rotational rheometer * = Phase angle δ at 0.1 MPa (G * =0.1 MPa) is 50 degrees or more, the molecular structure of the copolymer is a linear structure containing no long chain branches or a substantially linear structure containing a small amount of long chain branches that does not affect the mechanical strength. In addition, the absolute value of the complex modulus G measured by a rotational rheometer * = Phase angle δ at 0.1 MPa (G * = 0.1 MPa) is lower than 50 degrees, the molecular structure of the copolymer will contain excessive long chain branches, resulting in poor mechanical strength. Absolute value of complex modulus G measured by a rotational rheometer * The phase angle δ at G = 0.1 MPa is affected by both the molecular weight distribution and long chain branching. However, for copolymers with Mw / Mn ≦ 4, more preferably Mw / Mn ≦ 3, it is an index of the amount of long chain branching, and the more long chain branches there are in the molecular structure, the lower the δ(G *If the Mw / Mn of the copolymer is 1.5 or more, the δ(G * =0.1MPa) value never exceeds 75 degrees.

[0048] The method for measuring the complex elastic modulus is as follows. The sample is placed in a 1.0 mm thick heat press mold and preheated for 5 minutes in a heat press machine with a surface temperature of 180°C. The residual gas in the molten resin is degassed by repeatedly applying and depressurizing pressure, and then the sample is pressurized to 4.9 MPa and held for 5 minutes. The sample is then transferred to a press machine with a surface temperature of 25°C and cooled by holding at a pressure of 4.9 MPa for 3 minutes to create a press plate made of the sample with a thickness of approximately 1.0 mm. The press plate made of the sample is processed into a circle with a diameter of 25 mm to use as a sample. A Rheometrics ARES type rotational rheometer is used as a measuring device for dynamic viscoelastic properties, and dynamic viscoelasticity is measured under the following conditions in a nitrogen atmosphere. Plate: φ25mm parallel plate ·Temperature: 160℃ Distortion: 10% Measurement angular frequency range: 1.0×10 -2 ~1.0×10 2 rad / s Measurement interval: 5 points / decade Absolute value of complex elastic modulus G * Common logarithm logG of (Pa) * Plot the phase angle δ against logG * = 5.0, the value of δ (degrees) at the point * = 0.1MPa). * If there is no point corresponding to =5.0, logG * Using two points around =5.0, logG * The δ value at logG = 5.0 is calculated by linear interpolation. * <5, logG * Using the three largest values, we plot logG on a quadratic curve. * = 5.0.

[0049] - Copolymer production The copolymer according to the present invention is preferably produced in the presence of a transition metal catalyst, from the viewpoint of making the molecular structure thereof linear. Polymerization catalyst The type of polymerization catalyst used in the production of the copolymer according to the present invention is not particularly limited as long as it is capable of copolymerizing the structural unit (A), the structural unit (B), and the optional structural unit (C). For example, a transition metal compound of Groups 5 to 11 having a chelating ligand can be mentioned. Specific examples of preferred transition metals include vanadium atom, niobium atom, tantalum atom, chromium atom, molybdenum atom, tungsten atom, manganese atom, iron atom, platinum atom, ruthenium atom, cobalt atom, rhodium atom, nickel atom, palladium atom, copper atom, etc. Among these, preferred are transition metals of Groups 8 to 11, more preferred are transition metals of Group 10, and particularly preferred are nickel (Ni) and palladium (Pd). These metals may be used alone or in combination. Chelating ligands have at least two atoms selected from the group consisting of P, N, O, and S, and include ligands that are bidentate or multidentate, and are electronically neutral or anionic. Exemplary chelating ligand structures are given in the review by Brookhart et al. (Chem. Rev., 2000, 100, 1169). The chelating ligand preferably includes a bidentate anionic P, O ligand. Examples of the bidentate anionic P, O ligand include phosphorus sulfonic acid, phosphorus carboxylic acid, phosphorus phenol, and phosphorus enolate. Other examples of the chelating ligand include a bidentate anionic N, O ligand. Examples of the bidentate anionic N, O ligand include salicylaldimine and pyridine carboxylic acid. Other examples of the chelating ligand include a diimine ligand, a diphenoxide ligand, and a diamide ligand.

[0050] The structure of the metal complex obtained from the chelating ligand is represented by the following structural formula (a) or (b) in which an arylphosphine compound, an arylarsine compound or an arylantimony compound which may have a substituent is coordinated. [ka] [ka] [In structural formula (a) and structural formula (b), M represents a transition metal belonging to any of Groups 5 to 11 of the periodic table of the elements, that is, various transition metals as described above. X 1 represents oxygen, sulfur, -SO3-, or -CO2-. Y 1 represents carbon or silicon. n represents an integer of 0 or 1. E 1 represents phosphorus, arsenic or antimony. R 53 and R 54 each independently represents hydrogen or a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom. R 55 each independently represents hydrogen, halogen, or a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom. R 56 and R 57 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom, OR 52 , CO2R 52 , CO2M', C(O)N(R 51 )2, C(O)R 52 , S.R. 52 , SO2R 52 , SOR 52 , OSO2R 52 , P(O)(OR 52 ) 2-y (R 51 ) y , C.N., N.H.R. 52 , N(R 52)2, Si(OR 51 ) 3-x (R 51 ) x , OSi(OR 51 ) 3-x (R 51 ) x , NO2, SO3M', PO3M'2, P(O)(OR 52 )2M' or an epoxy-containing group. R 51 represents hydrogen or a hydrocarbon group having 1 to 20 carbon atoms. R 52 represents a hydrocarbon group having 1 to 20 carbon atoms. M′ represents an alkali metal, an alkaline earth metal, ammonium, a quaternary ammonium or a phosphonium; x represents an integer of 0 to 3; and y represents an integer of 0 to 2. In addition, R 56 and R 57 may be linked to each other to form an alicyclic ring, an aromatic ring, or a heterocyclic ring containing a heteroatom selected from oxygen, nitrogen, or sulfur, in which case the ring has 5 to 8 members and may or may not have a substituent on the ring. L 1 represents a ligand coordinated to M. Also, R 53 and L 1 may be bonded to each other to form a ring.

[0051] More preferably, it is a transition metal complex represented by the following structural formula (c). [ka] [In structural formula (c), M represents a transition metal belonging to any of Groups 5 to 11 of the periodic table of the elements, that is, various transition metals as described above. X 1 represents oxygen, sulfur, -SO3-, or -CO2-. Y 1 represents carbon or silicon. n represents an integer of 0 or 1. E 1represents phosphorus, arsenic or antimony. R 53 and R 54 each independently represents hydrogen or a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom. R 55 each independently represents hydrogen, halogen, or a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom. R 58 , R 59 , R 60 and R 61 each independently represents a hydrogen atom, a halogen atom, a hydrocarbon group having 1 to 30 carbon atoms which may contain a heteroatom, OR 52 , CO2R 52 , CO2M', C(O)N(R 51 )2, C(O)R 52 , S.R. 52 , SO2R 52 , SOR 52 , OSO2R 52 , P(O)(OR 52 ) 2-y (R 51 ) y , C.N., N.H.R. 52 , N(R 52 )2, Si(OR 51 ) 3-x (R 51 ) x , OSi(OR 51 ) 3-x (R 51 ) x , NO2, SO3M', PO3M'2, P(O)(OR 52 )2M' or an epoxy-containing group. R 51 represents hydrogen or a hydrocarbon group having 1 to 20 carbon atoms. R 52 represents a hydrocarbon group having 1 to 20 carbon atoms. M′ represents an alkali metal, an alkaline earth metal, ammonium, a quaternary ammonium or a phosphonium; x represents an integer of 0 to 3; and y represents an integer of 0 to 2. In addition, R 58 ~R 61may be bonded to each other to form an alicyclic ring, an aromatic ring, or a heterocyclic ring containing a heteroatom selected from oxygen, nitrogen, or sulfur. In this case, the number of ring members is 5 to 8, and the ring may or may not have a substituent. L 1 represents a ligand coordinated to M. Also, R 53 and L 1 may be bonded to each other to form a ring.

[0052] Here, typical catalysts of Group 5 to 11 transition metal compounds having a chelating ligand include so-called SHOP catalysts and Drent catalysts. The SHOP catalyst is a catalyst in which a phosphorus-based ligand having an aryl group which may have a substituent is coordinated to nickel metal (see, for example, WO2010-050256). Furthermore, the Drent catalyst is a catalyst in which a phosphorus-based ligand having an aryl group which may have a substituent is coordinated to palladium metal (see, for example, JP-A-2010-202647).

[0053] Copolymerization method: The polymerization method for the copolymer according to the present invention is not limited. Examples of the polymerization method include slurry polymerization in which at least a portion of the produced polymer becomes a slurry in a medium, bulk polymerization in which the liquefied monomer itself is used as the medium, gas phase polymerization in vaporized monomer, and high pressure ionic polymerization in which at least a portion of the produced polymer is dissolved in monomer liquefied at high temperature and pressure. The polymerization method may be any of batch polymerization, semi-batch polymerization, and continuous polymerization. Furthermore, living polymerization may be carried out, or polymerization may be carried out while simultaneously causing chain transfer. Furthermore, during polymerization, a so-called chain shuttling agent (CSA) may be used in combination to carry out a chain shuttling reaction or coordinate chain transfer polymerization (CCTP). Specific manufacturing processes and conditions are disclosed in, for example, Japanese Patent Application Laid-Open No. 2010-260913 and Japanese Patent Application Laid-Open No. 2010-202647.

[0054] Method for introducing carboxyl groups and / or dicarboxylic anhydride groups into copolymers: The method for introducing a carboxyl group and / or a dicarboxylic anhydride group into the copolymer according to the present invention is not particularly limited. Carboxyl groups and / or dicarboxylic anhydride groups can be introduced by various methods within the scope of the present invention. Examples of methods for introducing a carboxyl group and / or a dicarboxylic anhydride group include a method of directly copolymerizing a comonomer having a carboxyl group and / or a dicarboxylic anhydride group, and a method of copolymerizing another monomer and then introducing a carboxyl group and / or a dicarboxylic anhydride group by modification.

[0055] Methods for introducing a carboxyl group and / or a dicarboxylic anhydride group by modification include, for example, when introducing a carboxylic acid, a method in which an acrylic ester is copolymerized and then hydrolyzed to convert it to a carboxylic acid, and a method in which t-butyl acrylate is copolymerized and then thermally decomposed to convert it to a carboxylic acid.

[0056] A conventionally known acid-base catalyst may be used as an additive for promoting the reaction during the hydrolysis or thermal decomposition. The acid-base catalyst is not particularly limited, and examples of the acid-base catalyst that can be used include, for example, hydroxides of alkali metals or alkaline earth metals such as sodium hydroxide, potassium hydroxide, or lithium hydroxide, alkali metals or carbonates of alkaline earth metals such as sodium hydrogencarbonate or sodium carbonate, solid acids such as montmorillonite, inorganic acids such as hydrochloric acid, nitric acid, or sulfuric acid, and organic acids such as formic acid, acetic acid, benzoic acid, citric acid, paratoluenesulfonic acid, trifluoroacetic acid, or trifluoromethanesulfonic acid. From the viewpoints of reaction promotion effect, cost, equipment corrosivity, etc., sodium hydroxide, potassium hydroxide, sodium carbonate, trifluoroacetic acid, and paratoluenesulfonic acid are preferred, and trifluoroacetic acid and paratoluenesulfonic acid are more preferred.

[0057] (5) Ionomer The ionomer according to the present invention is an ionomer having a substantially linear structure in which at least a part of the carboxyl group and / or dicarboxylic anhydride group of the structural unit (B) of the copolymer of the present invention is converted to a metal-containing carboxylate containing at least one metal ion selected from Group 1, Group 2, or Group 12 of the periodic table. As described below, the ionomer is obtained by reacting an ionomer base resin with a metal salt, and during this process, a reaction that cuts the molecular chain of the polymer does not usually occur. Therefore, parameters related to the structure, such as the molar ratio of the comonomer, the degree of branching, and randomness, are usually preserved between the ionomer base resin and the ionomer.

[0058] -Ionomer structure The ionomer according to the present invention has a substantially linear structure like the copolymer according to the present invention, and therefore the absolute value of the complex modulus G measured by a rotational rheometer * The phase angle δ at pressure σ=0.1 MPa is 50 to 75 degrees. The lower limit of the phase angle δ may be 51 degrees or more, and the upper limit of the phase angle δ may be 64 degrees or less. Phase angle δ(G * =0.1MPa) is lower than 50 degrees, the molecular structure of the ionomer contains excessive long chain branches, resulting in poor mechanical strength. As mentioned above, if Mw / Mn≦4, the phase angle δ is an index of the amount of long chain branches. If the Mw / Mn of an ionomer is 1.5 or more, the phase angle δ(G * =0.1MPa) value never exceeds 75 degrees.

[0059] Melting point of ionomer (Tm, °C) The melting point (Tm, °C) of the ionomer according to the present invention is preferably 50° C. to 140° C., more preferably 60° C. to 138° C., and most preferably 70° C. to 135° C. If it is lower than this range, the heat resistance is insufficient, and if it is higher than this range, the adhesiveness may be poor. Of the ionomers related to the present invention, ionomers based on a binary copolymer consisting only of structural unit (A) and structural unit (B) have a melting point of 90°C or higher, preferably 95°C or higher, and more preferably 100°C or higher, while ionomers based on a ternary or higher multi-component copolymer have a melting point of less than 100°C, preferably less than 95°C, and more preferably less than 90°C.

[0060] Crystallinity (%): In the ionomer of the present invention, the crystallinity observed by differential scanning calorimetry (DSC) is not particularly limited, but is preferably greater than 0% and not greater than 30%, more preferably greater than 0% and not greater than 25%, particularly preferably greater than 5% and not greater than 25%, and most preferably 7% or more and not greater than 24%. If the crystallinity is 0%, the toughness of the ionomer is insufficient, and if the crystallinity is higher than 30%, the transparency of the copolymer may be poor. Note that the crystallinity is an index of transparency, and it can be determined that the lower the crystallinity of the ionomer, the more excellent its transparency.

[0061] Metal ions The metal ions contained in the ionomer of the present invention are not particularly limited, and may include metal ions used in conventionally known ionomers. Among them, metal ions of Groups 1, 2, or 12 of the periodic table are preferred, and Li + , Na + , K + , Rb + , Cs + , Mg 2+ , Ca 2+ , Sr 2+ , B.A. 2+ and Zn 2+More preferably, at least one selected from the group consisting of Li + , Na + , K + , Mg 2+ , Ca 2+ , and Zn 2+ , more preferably Na + , and Zn 2+ At least one selected from the group consisting of: Two or more of these metal ions may be mixed and contained as necessary.

[0062] ·Neutralization degree (mol%) The metal ion content is preferably an amount that neutralizes at least a part or all of the carboxyl groups and / or dicarboxylic anhydride groups in the copolymer as the base polymer, and the preferred degree of neutralization (average degree of neutralization) is 5 to 95 mol%, more preferably 10 to 90 mol%, and even more preferably 20 to 80 mol%. A high degree of neutralization results in an ionomer with high tensile strength and tensile stress at break, and low tensile strain at break, but the melt flow rate (MFR) of the ionomer tends to be low. On the other hand, a low degree of neutralization results in an ionomer with a moderate MFR, but low tensile modulus and tensile stress at break, and high tensile strain at break. The degree of neutralization can be determined from the ratio of the total molar amount of the valence×molar amount of the metal ion to the total molar amount of the carboxy groups that may be contained in the carboxy groups and / or dicarboxylic anhydride groups in the copolymer. When a dicarboxylic anhydride group forms a carboxylate, it opens its ring to form a dicarboxylic acid, so the total molar amount of the carboxyl groups is calculated assuming that there are 2 mol of carboxyl groups per 1 mol of dicarboxylic anhydride group. 2+ For divalent metal ions such as those mentioned above, 1 mole of each can form a salt with 2 moles of carboxyl groups, and the total molar amount of molecules with the degree of neutralization is calculated by 2 x the molar amount.

[0063] -Ionomer manufacturing method The ionomer according to the present invention may be obtained by subjecting a copolymer of ethylene and / or an α-olefin having 3 to 20 carbon atoms / unsaturated carboxylic acid obtained by the above-mentioned method for introducing a carboxyl group and / or a dicarboxylic anhydride group into the copolymer to a conversion step of treating the copolymer with a metal salt containing at least one metal ion selected from Group 1, Group 2, or Group 12 of the periodic table to convert the copolymer into a metal-containing carboxylate. The ionomer according to the present invention may also be obtained by subjecting a copolymer of ethylene and / or an α-olefin having 3 to 20 carbon atoms / unsaturated carboxylic acid ester to a heat conversion step of heating the copolymer to convert at least a part of the ester groups in the copolymer into a metal-containing carboxylate containing at least one metal ion selected from Group 1, Group 2, or Group 12 of the periodic table.

[0064] When an ionomer is produced after introducing a carboxyl group and / or a dicarboxylic anhydride group into a polymer, the production method is, for example, as follows: A metal ion source is prepared by kneading a metal salt with a substance that captures metal ions, such as an ethylene / methacrylic acid (MAA) copolymer, optionally with heating, and then the metal ion source is added to an ionomer base resin in an amount that results in a desired degree of neutralization, followed by kneading.

[0065] In the thermal conversion step, (i) ethylene and / or an α-olefin having 3 to 20 carbon atoms / unsaturated carboxylic acid ester copolymer may be heated to convert the copolymer into an ethylene and / or an α-olefin having 3 to 20 carbon atoms / unsaturated carboxylic acid copolymer by hydrolysis or thermal decomposition, and then the copolymer may be reacted with a compound containing a metal ion of Group 1, Group 2, or Group 12 of the periodic table to convert the carboxylic acid in the copolymer into the metal-containing carboxylate. In addition, (ii) ethylene and / or an α-olefin having 3 to 20 carbon atoms / unsaturated carboxylic acid ester copolymer may be heated to convert the ester group of the copolymer into the metal-containing carboxylate while reacting the copolymer with a compound containing a metal ion of Group 1, Group 2, or Group 12 of the periodic table to convert the ester group portion in the copolymer into the metal-containing carboxylate.

[0066] Furthermore, the compound containing a metal ion may be an oxide, hydroxide, carbonate, bicarbonate, acetate, formate, etc. of a metal of Group 1, 2, or 12 of the periodic table. The compound containing metal ions may be supplied to the reaction system in the form of particles or fine powder, or may be dissolved or dispersed in water or an organic solvent and then supplied to the reaction system, or a master batch may be prepared using an ethylene / unsaturated carboxylic acid copolymer or an olefin copolymer as a base polymer and then supplied to the reaction system. In order to ensure smooth reaction, it is preferable to prepare a master batch and supply it to the reaction system.

[0067] Furthermore, the reaction with the compound containing metal ions may be carried out by melt kneading using various types of equipment such as a vent extruder, a Banbury mixer, a roll mill, etc., and the reaction may be a batch or continuous method. Since the reaction can be carried out smoothly by discharging water and carbon dioxide gas by-produced by the reaction using a degassing device, it is preferable to carry out the reaction continuously using an extruder equipped with a degassing device such as a vent extruder. In the reaction with the compound containing metal ions, a small amount of water may be injected to promote the reaction.

[0068] The temperature at which the ethylene and / or C3-20 α-olefin / unsaturated carboxylic acid ester copolymer is heated may be any temperature at which the ester becomes a carboxylic acid, and if the heating temperature is too low, the ester is not converted to a carboxylic acid, whereas if the heating temperature is too high, decarbonylation or decomposition of the copolymer may proceed. Therefore, the heating temperature in the present invention is preferably in the range of 80°C to 350°C, more preferably 100°C to 340°C, even more preferably 150°C to 330°C, and even more preferably 200°C to 320°C.

[0069] The reaction time varies depending on the heating temperature, the reactivity of the ester group portion, etc., but is usually 1 minute to 50 hours, more preferably 2 minutes to 30 hours, even more preferably 2 minutes to 10 hours, still more preferably 2 minutes to 3 hours, and particularly preferably 3 minutes to 2 hours.

[0070] In the above steps, the reaction atmosphere is not particularly limited, but it is generally preferable to carry out the reaction under an inert gas flow. Examples of the inert gas include nitrogen, argon, and carbon dioxide. A small amount of oxygen or air may be mixed in.

[0071] The reactor used in the above step is not particularly limited, and any method can be used as long as it can substantially uniformly stir the copolymer. A glass vessel or an autoclave (AC) equipped with a stirrer may be used, or any conventionally known kneading machine such as a Brabender plastograph, a single-screw or twin-screw extruder, a high-intensity screw-type kneader, a Banbury mixer, a kneader, or a roll may be used.

[0072] Whether or not a metal ion has been introduced into an ionomer-based resin and it has become an ionomer can be confirmed by measuring the IR spectrum of the resulting resin and examining the decrease in the peak derived from the carbonyl group of the carboxylic acid (dimer). Similarly, the degree of neutralization can be confirmed by calculating from the molar ratio described above, as well as examining the decrease in the peak derived from the carbonyl group of the carboxylic acid (dimer) and the increase in the peak derived from the carbonyl group of the carboxylate salt group.

[0073] <Ionomer properties> The ionomer used in the present invention, particularly the ionomer suitable for laminating, has any one or a combination of the following physical properties under the measurement conditions described in the Examples section below. MFR: In the ionomer of the present invention, the melt flow rate (MFR) at a temperature of 190° C. under a load of 2.16 kg is 0.01 to 30 g / 10 min, preferably 0.1 to 15 g / 10 min, and more preferably 0.5 to 20 g / 10 min. When the MFR of the ionomer is within this range, laminate molding is easy.

[0074] Tensile modulus: In the ionomer of the present invention, the tensile modulus is 20 MPa or more, preferably 20 to 350 MPa, and more preferably 20 to 300 MPa. When the tensile modulus of the ionomer is within this range, the adhesion when formed into a laminate is good, and the ionomer can be produced without difficulty in designing the modulus of elasticity.

[0075] Tensile impact strength: The ionomer of the present invention has a tensile impact strength of 100 KJ / m 2 More than 700KJ / m, preferably tensile impact strength is 700KJ / m 2 More preferably, it is 800KJ / m or more. 2 That's all. Ionomers based on ternary or higher multi-component copolymers, especially those with a tensile impact strength of 700KJ / m 2 It is possible to obtain an ionomer that achieves the above. If the tensile impact strength of the ionomer is in this range, the risk of breakage is small even if it is rubbed, etc. There is no particular upper limit for the tensile impact strength as long as it is within the range that can be obtained from the materials used by those skilled in the art.

[0076] ·Resin composition Although the (X1) ionomer in the present invention can be extrusion laminated by itself due to ionic crosslinking, it may be further processed to improve the processability during extrusion laminate processing by adding (X2) an ethylene copolymer having ethylene as an essential monomer by high pressure radical polymerization to form a polymer composition. The "polymer composition" here includes a composition in which the weight ratio of (X1) ionomer is 100% by weight, that is, a material consisting of (X1) ionomer alone.

[0077] In the present invention, the weight ratio of the ionomer (X1) in the polymer composition is 100 to 60% by weight. By making the weight ratio 60% by weight or more, physical properties such as high hot tack strength can be more easily obtained.

[0078] (X2) is an ethylene copolymer obtained by high pressure radical polymerization and containing ethylene as an essential monomer. It is a low density polyethylene (hereinafter referred to as LDPE) obtained by a high pressure radical polymerization process, or an ethylene copolymer consisting of ethylene and a radical polymerizable monomer other than ethylene. When (X2) contains a radical polymerizable monomer other than ethylene obtained by high pressure radical polymerization, the amount of ethylene structural units in (X2) is preferably 75 mol% or more, more preferably 80 mol% or more of the whole of (X2). By setting it in this range, the melt tension of the polymer composition becomes an appropriate range, which makes it easier to perform extrusion lamination molding, etc.

[0079] Examples of radical polymerizable monomers other than ethylene include vinyl esters such as vinyl propionate, vinyl acetate, vinyl caproate, vinyl caprylate, vinyl laurate, vinyl stearate, and vinyl trifluoroacetate, and α,β-unsaturated carboxylic acids or ester derivatives thereof such as acrylic acid, methacrylic acid, methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, propyl acrylate, propyl methacrylate, isopropyl acrylate, isopropyl methacrylate, n-butyl acrylate, n-butyl methacrylate, cyclohexyl acrylate, cyclohexyl methacrylate, lauryl acrylate, lauryl methacrylate, stearyl acrylate, and stearyl methacrylate. Among these, particularly preferred are (meth)acrylic acid and its alkyl esters such as methyl ester and ethyl ester.

[0080] The MFR of low-density polyethylene (LDPE) obtained by the high-pressure radical polymerization process is selected in the range of 0.05 to 50 g / 10 min, preferably 0.1 to 30 g / 10 min. Within this range, the melt tension of the polymer composition is in an appropriate range, making extrusion lamination molding and the like easy.

[0081] The density of the LDPE is 0.91 to 0.94 g / cm 3 , preferably 0.912 to 0.935 g / cm 3 , and more preferably 0.912 to 0.930 g / cm 3 The molecular weight distribution (Mw / Mn) is selected within the range of 3.0 to 12, and preferably 4.0 to 12.0.

[0082] The (meth)acrylic acid and (meth)acrylic acid ester content in the ethylene copolymer obtained by the high pressure radical polymerization process is in the range of 3 to 20% by weight, preferably 5 to 15% by weight. The MFR of these copolymers is selected in the range of 0.1 to 30 g / 10 min, preferably 0.2 to 20 g / 10 min. If the MFR is within this range, the melt tension of the composition will be in an appropriate range, and extrusion lamination molding and the like will be easy.

[0083] The LDPE and ethylene copolymers are produced by a known high pressure radical polymerization method, and may be produced by either a tubular method or an autoclave method.

[0084] In the present invention, the weight ratio of the ethylene copolymer (X2) produced by high pressure radical polymerization and having ethylene as an essential monomer in the polymer composition is 0 to 40% by weight. By making it 40% by weight or less, it is possible to improve the processability during molding processing, while easily obtaining physical properties such as high hot tack strength due to the ionomer of the (X1) component.

[0085] The melt flow rate (MFR) of the polymer composition of the present invention is in the range of 1.0 to 100 g / 10 min, preferably in the range of 2.0 to 50 g / 10 min, and more preferably in the range of 2.0 to 20 g / 10 min. By setting the MFR in the above range, good molding processability can be obtained, such as keeping the extrusion load low and improving the extensibility, and the neck-in does not become large, and the stability of the film during film formation is improved.

[0086] The polymer composition of the present invention can be blended by a known method generally used as a conventional resin composition blending method. One example of the method is to simply dry blend the (X1) component, the (X2) component, and other additives that can be added. Another example is to dry blend the (X1) component, the (X2) component, and various additives as desired using a mixer such as a tumbler, a ribbon blender, or a Henschel mixer, and then melt mix them using a known continuous melt kneader such as a single screw extruder or a twin screw extruder, and extrude them to prepare pellets, thereby obtaining the polymer composition.

[0087] To the polymer composition of the present invention, known additives such as antifogging agents, organic or inorganic fillers, antioxidants, organic or inorganic pigments, ultraviolet protection agents, lubricants such as saturated or unsaturated fatty acid amides and metal salts of saturated or unsaturated higher fatty acids, dispersants, nucleating agents, crosslinking agents, etc. may be added within a range that does not essentially impair the properties of the present invention.

[0088] <Laminate> The laminate of the present invention is a laminate including at least Layer I, which is a substrate layer, and Layer II, which is a sealant layer. In some cases, a layer such as a polyolefin layer, such as polyethylene, called polylami, or an acid-modified polyolefin layer obtained by graft-modifying various polyolefins and / or rubbers with unsaturated carboxylic acid or its derivatives, may be provided between the substrate layer and the sealant layer, or on the outside of the substrate layer. In addition, the substrate may be subjected to a deposition treatment, a polyvinylidene chloride coating, or the like.

[0089] Examples of the substrate layer which is the I layer in the laminate of the present invention include paper such as fine paper, craft paper, tissue paper, and Kent paper, metal foil such as aluminum foil, cellophane, woven fabric, nonwoven fabric, nylon substrates such as stretched nylon, non-stretched nylon, special nylon (MXD6, etc.), and K-nylon (polyvinylidene fluoride coated), PET (polyethylene terephthalate) substrates such as stretched PET, non-stretched PET, K-PET, and aluminum-deposited PET (VMPET), polypropylene substrates such as stretched PP (OPP), non-stretched PP (CPP), aluminum-deposited PP, K-PP, and co-extruded PP film, and synthetic resin film substrates such as LDPE film, LLDPE, EVA film, stretched LDPE film, stretched HDPE film, and polystyrene film. The substrate layer which is the I layer may also be a composite substrate in which the above-listed substrates are bonded together in advance by known dry lamination or extrusion lamination. Examples of such composite substrates include stretched nylon / stretched PET, stretched PET / aluminum foil / stretched PET, stretched PET / LDPE / aluminum foil, stretched PET / LDPE / aluminum foil / LDPE, stretched PET / saponified ethylene-vinyl acetate copolymer, stretched polypropylene / saponified ethylene-vinyl acetate copolymer, etc. These may also be printed.

[0090] The polymer composition for lamination of the present invention is used for the sealant layer, which is the second layer in the laminate of the present invention. In addition to the polymer composition of the present invention, any known resin material used in conventional polymer resin compositions for lamination may be blended into the sealant layer within a range that does not impair the effects of the present invention. Examples of such materials include high-density polyethylene, medium-density polyethylene, low-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-acrylic acid ester copolymer, and other ionomers. The blending amount of the resin composition can be selected arbitrarily from 1 to 50% by weight, preferably 5 to 20% by weight. The resin composition may be a mixture of two or more materials. The sealant layer is preferably a layer composed only of the polymer composition of the present invention.

[0091] The method for producing the laminate of the present invention may be carried out by various known methods, including a method in which the sealant layer, which is the second layer, is processed into a film form by film molding in advance, and the second layer, which is a film, is laminated by laminating it to the substrate of the first layer by dry lamination molding, or a method in which the second layer, which is a film, is used as a sandwich substrate for the substrate of the first layer by extrusion lamination molding using a resin that can be extrusion laminated, such as LDPE or an ethylene copolymer, or a method in which a polymer composition for lamination is extruded as the second layer by extrusion lamination molding and laminated on the substrate of the first layer by extrusion lamination molding. When the sealant layer of the laminate of the present invention is directly extruded by extrusion lamination molding to laminate, it is not particularly limited, but it is preferable to perform molding at a molding resin temperature of 250 to 290 ° C and a cooling roll temperature of 10 to 25 ° C, particularly in the case of the polymer composition for lamination of the present invention.

[0092] The laminate of the present invention has a sealant layer that is excellent in hot tack properties due to the substantially linear ionomer, and is therefore suitable for use as a packaging material in the form of a bag. EXAMPLES

[0093] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples. The physical properties in the examples and comparative examples were measured and evaluated by the methods shown below. In the tables, "no data" means that no measurement was performed, and "not detected" means that the value was below the detection limit.

[0094] <Measurement and Evaluation> (1) Absolute value of complex elastic modulus G * Measurement of phase angle δ at 0.1 MPa 1) Sample preparation and measurement The sample was placed in a 1.0 mm thick mold for hot pressing, preheated in a hot press machine with a surface temperature of 180°C for 5 minutes, and then repeatedly pressurized and depressurized to remove residual gas in the molten resin. The sample was then pressed at 4.9 MPa and held for 5 minutes. The sample was then transferred to a press machine with a surface temperature of 25°C and cooled by holding at a pressure of 4.9 MPa for 3 minutes to produce a pressed plate made of a sample with a thickness of approximately 1.0 mm. The pressed plate made of the sample was processed into a circular shape with a diameter of 25 mm to prepare a sample. The dynamic viscoelasticity was measured under the following conditions in a nitrogen atmosphere using an ARES type rotational rheometer manufactured by Rheometrics Co., Ltd. as a measuring device for dynamic viscoelastic properties. Plate: φ25mm (diameter) parallel plate ·Temperature: 160℃ Distortion: 10% Measurement angular frequency range: 1.0×10 -2 ~1.0×10 2 rad / s Measurement interval: 5 points / decade Absolute value of complex elastic modulus G * Common logarithm logG of (Pa) * Plot the phase angle δ against logG * = 5.0, the value of δ (degrees) at the point * = 0.1MPa). * If there is no point corresponding to =5.0, logG * Using two points around =5.0, logG * The δ value at logG = 5.0 was calculated by linear interpolation.* <5, logG * Using the three largest values, we plot logG on a quadratic curve. * The δ value at =5.0 was extrapolated.

[0095] (2) Measurement of weight average molecular weight (Mw) and molecular weight distribution parameter (Mw / Mn) The weight average molecular weight (Mw) was determined by gel permeation chromatography (GPC). The molecular weight distribution parameter (Mw / Mn) was calculated from the ratio of Mw to Mn, Mw / Mn, obtained by further determining the number average molecular weight (Mn) by gel permeation chromatography (GPC). The measurements were carried out according to the following procedures and conditions.

[0096] 1) Sample pretreatment When the sample contained a carboxylic acid group, it was subjected to an esterification treatment, such as methyl esterification using diazomethane or trimethylsilyl (TMS) diazomethane, before use in the measurement. When the sample contained a carboxylate group, it was subjected to an acid treatment to modify the carboxylate group to a carboxylic acid group, and then subjected to the above-mentioned esterification treatment before use in the measurement.

[0097] 2) Preparation of sample solution 3 mg of sample and 3 mL of o-dichlorobenzene were weighed into a 4 mL vial, and the vial was capped with a screw cap and a Teflon (registered trademark) septum, and then shaken for 2 hours at 150°C using a Senshu Scientific SSC-7300 high-temperature shaker. After shaking, it was visually confirmed that there were no insoluble components.

[0098] 3) Measurement A Waters Alliance GPCV2000 was connected to Showa Denko's high temperature GPC columns Showdex HT-G x 1 and HT-806M x 2, and measurements were performed using o-dichlorobenzene as the eluent at a temperature of 145°C and a flow rate of 1.0 mL / min.

[0099] 4) Calibration curve The column was calibrated using monodisperse polystyrene (S-7300, S-3900, S-1950, S-1460, S-1010, S-565, S-152, S-66.0, S-28.5, S-5.05, each 0.07 mg / ml solution) manufactured by Showa Denko, n-eicosane and n-tetracontane were measured under the same conditions as above, and the elution time and the logarithm of the molecular weight were approximated by a fourth-order equation. PS ) and polyethylene molecular weight (M PE The following formula was used to convert M PE =0.468×M PS

[0100] (3) Melt flow rate (MFR) The MFR was measured in accordance with Table 1-Condition 7 of JIS K-7210 (1999) at a temperature of 190°C and a load of 21.18N (=2.16kg).

[0101] (4) Tensile test A 1 mm thick sheet was prepared as a sample by the method described in JIS K7151 (1995) (cooling method A), and this was punched out to prepare a small 5B type test piece described in JIS K7162 (1994). A tensile test was performed at a temperature of 23°C in accordance with JIS K7161 (1994) to measure the tensile modulus, tensile stress at break, and tensile strain at break. The test speed was 10 mm / min.

[0102] (5) Melting point and crystallinity The melting point is indicated by the peak temperature of the endothermic curve measured by a differential scanning calorimeter (DSC). The measurement was performed using a DSC (DSC7020) manufactured by SII Nano Technology Co., Ltd. under the following measurement conditions. Approximately 5.0 mg of the sample was packed into an aluminum pan, heated to 200°C at 10°C / min, held at 200°C for 5 minutes, and then cooled to 30°C at 10°C / min. After holding at 30°C for 5 minutes, the sample was again heated at 10°C / min. The maximum peak temperature in the absorption curve was taken as the melting point Tm, and the heat of fusion (ΔH) was calculated from the area of ​​the melting endothermic peak. The degree of crystallinity (%) was calculated by dividing the heat of fusion by the heat of fusion of perfect crystals of high density polyethylene (HDPE), 293 J / g.

[0103] (6) Method for measuring the amount of structural units derived from monomers having a carboxyl group and / or a dicarboxylic anhydride group, and non-cyclic monomers, and the number of branches per 1,000 carbon atoms The amount of structural units derived from monomers having a carboxy group and / or a dicarboxylic anhydride group and non-cyclic monomers in the copolymer of the present invention, and the number of branches per 1,000 carbon atoms are 13 It can be determined using C-NMR spectroscopy. 13 C-NMR was measured by the following method. 200-300 mg of sample was placed in an NMR sample tube with an inner diameter of 10 mm together with 2.4 ml of a mixed solvent of o-dichlorobenzene (C6H4Cl2) and deuterated bromide benzene (C6D5Br) (C6H4Cl2 / C6D5Br = 2 / 1 (volume ratio)) and hexamethyldisiloxane, a chemical shift standard substance, and the tube was purged with nitrogen, sealed, and heated to dissolve and prepare a homogeneous solution to be used as the NMR measurement sample. NMR measurements were performed at 120°C using an AV400M NMR instrument from Bruker Japan equipped with a 10 mmφ cryoprobe. 13 C-NMR was measured using the inverse gate decoupling method with a sample temperature of 120°C, a pulse angle of 90°, a pulse interval of 51.5 seconds, and an accumulation number of 512 or more. The chemical shifts are those of hexamethyldisiloxane. 13 The C signal was set at 1.98 ppm, and the other 13 The chemical shifts of the C signals were based on this.

[0104] 1) Sample pretreatment When the sample contained a carboxylate group, the sample was subjected to an acid treatment to convert the carboxylate group to a carboxyl group before the measurement. When the sample contained a carboxyl group, an esterification treatment such as methyl esterification using diazomethane or trimethylsilyl (TMS) diazomethane may be appropriately performed.

[0105] 2) Calculation of the amount of structural units derived from monomers having a carboxy group and / or a dicarboxylic anhydride group, and non-cyclic monomers <e tba> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 It is detected at 79.6 to 78.8 in the C-NMR spectrum. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I(tBA) × 100 / 〔I(tBA) + I(E)〕 Here, I(tBA) and I(E) are the quantities shown in the following formulas. I(tBA)=I 79.6~78.8 I(E)=(I 180.0~135.0 +I 120.0~5.0 -I(tBA) × 7) / 2

[0106] <e tba nb> The quaternary carbon signal of the t-butyl acrylate group of tBA is 13 The methine carbon signal of NB was detected at 41.9 to 41.1 ppm in the C-NMR spectrum. Using these signal intensities, the amount of comonomer was calculated from the following formula. Total amount of tBA (mol%) = I(tBA) × 100 / 〔I(tBA) + I(NB) + I(E)〕 Total amount of NB (mol%) = I(NB) × 100 / 〔I(tBA) + I(NB) + I(E)〕 Here, I(tBA), I(NB), and I(E) are quantities expressed by the following formulas. I(tBA)=I 79.6~78.8 I(NB)=(I 41.9~41.1 ) / 2 I(E)=(I 180.0~135.0 +I 120.0~5.0 -I(NB) x 7 -I(tBA) x 7) / 2

[0107] In addition, when the structural unit amount of each monomer is indicated by "<0.1" including an inequality sign, it means that it is present as a structural unit in the copolymer, but the amount is less than 0.1 mol %, taking into account significant digits.

[0108] 3) Calculation of the number of branches per 1,000 carbon atoms Copolymers come in three types: isolated types, in which a branch exists alone in the main chain, complex types (face-to-face types in which branches face each other via the main chain, branched-branch types, in which there are branches within a branched chain, and chain types). The following is an example of the structure of an ethyl branch. In the example of the facing type, R represents an alkyl group.

[0109] [ka]

[0110] The number of branches per 1,000 carbons is calculated by substituting either I(B1), I(B2), or I(B4) below into the I (branch) term in the following formula. B1 represents methyl branches, B2 represents ethyl branches, and B4 represents butyl branches. The number of methyl branches is calculated using I(B1), the number of ethyl branches using I(B2), and the number of butyl branches using I(B4). Number of branches (per 1,000 carbons) = I (branches) x 1000 / I (total) Here, I(total), I(B1), I(B2), and I(B4) are quantities expressed by the following formulas. I(total)=I 180.0~135.0 +I 120.0~5.0 I(B1)=(I 20.0~19.8 +I 33.2~33.1 +I 37.5~37.3 ) / 4 I(B2)=I 8.6~7.6 +I 11.8~10.5 I(B4)=I 14.3~13.7 -I 32.2~32.0 Here, I is the integrated intensity, and the subscripts of I indicate the range of chemical shifts. For example, I 180.0~135.0 was detected between 180.0 ppm and 135.0 ppm. 13 C The integrated intensity of the signal is shown. The attribution was based on the non-patent literature Macromolecules 1984, 17, 1756-1761 and Macromolecules 1979, 12, 41. In addition, when the number of branches is indicated as "<0.1" including an inequality sign, it means that it exists as a structural unit in the copolymer, but the amount is less than 0.1 mol% considering significant figures. Also, "not detected" means below the detection limit.

[0111] (7) Infrared absorption spectrum The sample was melted at 180° C. for 3 minutes and compression molded to prepare a film with a thickness of about 50 μm. This film was analyzed by Fourier transform infrared spectroscopy to obtain an infrared absorption spectrum. Product name: FT / IR-6100 manufactured by JASCO Corporation Measurement method: transmission method Detector: TGS (Triglycine sulfate) Number of times: 16 to 512 Resolution: 4.0cm -1 Measurement wavelength: 5000~500cm -1

[0112] (8) Tensile impact strength 1) How to prepare samples for tensile impact strength test The sample was placed in a 1 mm thick mold for hot pressing, preheated for 5 minutes in a hot press machine with a surface temperature of 180 ° C., and then repeatedly pressurized and depressurized to melt the sample and degas the residual gas in the sample, and then pressurized at 4.9 MPa and held for 5 minutes. After that, while applying a pressure of 4.9 MPa, the sample was gradually cooled at a rate of 10 ° C. / min, and when the temperature had dropped to near room temperature, the molded plate was removed from the mold. The obtained molded plate was conditioned for more than 48 hours in an environment with a temperature of 23 ± 2 ° C. and a humidity of 50 ± 5 ° C. A test piece in the shape of ASTM D1822 Type-S was punched out from the conditioned press plate to prepare a tensile impact strength test sample.

[0113] 2) Tensile impact strength test conditions The tensile impact strength was measured using the above test pieces with reference to JIS K 7160-1996 B method. The only difference from JIS K 7160-1996 was the shape of the test pieces. Other measurement conditions were performed in accordance with JIS K 7160-1996.

[0114] (9) Adhesive strength The obtained laminate was cut into 15 mm widths along the molding flow direction, and the adhesive strength was measured by T-peel at a speed of 50 mm / min using a Tensilon (manufactured by Toyo Seiki Co., Ltd.) tensile tester. The adhesive strength was expressed in units of N / 15 mm.

[0115] (10) Hot tack strength Using a Lakotool hot tack tester SL-10, hot tack strength was measured in accordance with ASTM F1921-98 under the following conditions: sealing temperature 110-140°C, sealing pressure 0.414MPa, sealing time 1000ms, peel speed 200cm / min. The peel strength 500ms after sealing was completed was taken as the hot tack strength.

[0116] [Example 1] <Synthesis of metal complexes> (1) Synthesis of B-27DM / Ni complex The B-27DM / Ni complex was prepared according to Synthesis Example 4 described in WO 2010 / 050256, using the following 2-bis(2,6-dimethoxyphenyl)phosphano-6-pentafluorophenylphenol ligand (B-27DM). A nickel complex (B-27DM / Ni) was synthesized in which B-27DM and Ni(COD)2 reacted in a 1:1 ratio using bis(1,5-cyclooctadiene)nickel(0) (referred to as Ni(COD)2) according to Example 1 of WO 2010 / 050256. [ka]

[0117] <(Production Example 1): Production of ionomer-based resin precursor> An ethylene / tBu acrylate / norbornene copolymer was produced using a transition metal complex (B-27DM / Ni complex or B-423 / Ni complex). The copolymer was produced with reference to Production Example 1 or Production Example 3 described in JP 2016-79408 A. The production conditions and production results, which were appropriately changed such as the metal catalyst type, metal catalyst amount, trioctyl aluminum (TNOA) amount, toluene amount, comonomer type, comonomer amount, ethylene partial pressure, polymerization temperature, and polymerization time, are shown in Table 1, and the physical properties of the obtained copolymer are shown in Table 2.

[0118] [Table 1]

[0119] [Table 2]

[0120] <Production of ionomer-based resin> Internal volume 1.6m 3 In a SUS316L autoclave equipped with an agitator, 100 kg of the copolymer of Production Example 1, 2.0 kg of paratoluenesulfonic acid monohydrate, and 173 L of toluene were added and stirred at 105°C for 4 hours. 173 L of ion-exchanged water was added, stirred, and allowed to stand, and then the aqueous layer was extracted. Thereafter, the addition and withdrawal of ion-exchanged water was repeated until the pH of the extracted aqueous layer reached 5 or more. The remaining solution was added to a twin-screw extruder (L / D=42) equipped with a 42 mmφ vent device, and the solvent was distilled off by drawing a vacuum through the vent. Furthermore, the resin extruded continuously in the form of a strand from the die at the tip of the extruder was cooled in water and cut with a cutter to obtain resin pellets. In the IR spectrum of the obtained resin, the 850 cm -1 The disappearance of the peak near 1730 cm -1 The decrease in the peak near 1700 cm originates from the carbonyl group of the carboxylic acid (dimer). -1 An increase in the peak near As a result, decomposition of t-Bu ester and generation of carboxylic acid were confirmed, and ionomer base resin 1 was obtained. The physical properties of the obtained resin are shown in Tables 3 and 4. In the following tables, "E", "AA", and "NB" are abbreviations for "ethylene", "acrylic acid", and "norbornene", respectively, as structural units contained in the base resin.

[0121] [Table 3]

[0122] [Table 4]

[0123] <Ionomer production> 1) Preparation of Zn ion source Ethylene / methacrylic acid (MAA) copolymer (Mitsui Dow Polychemicals, brand: Nucrel N1050H) was continuously fed into a Toshiba Machine 26mmφ vented twin screw extruder (L / D=64) with a blending ratio of 54.5wt%, zinc oxide 45wt%, and zinc stearate 0.5wt%, and extruded under kneading conditions of barrel set temperature 150℃ and screw rotation speed 150rpm while removing gas and water generated during kneading from the vent part with a vacuum pump. Furthermore, the resin extruded continuously in the form of strands from the die at the tip of the extruder was cooled in water and cut with a cutter to obtain pellets as a Zn ion source.

[0124] 2): Preparation of ionomer Resin 1 and a Zn ion source were continuously fed into a Toshiba Machine twin-screw extruder (L / D=65) equipped with a 26mmφ vent device in a blending ratio that would give the desired degree of neutralization, and extrusion was performed under kneading conditions of barrel setting temperature 200°C and screw rotation speed 150 rpm, while injecting water at a ratio of 4 parts per 100 parts of the resin fed and removing gas and water generated during kneading from the vent part with a vacuum pump. Furthermore, the resin continuously extruded in the form of strands from the die at the tip of the extruder was cooled in water and cut with a cutter to obtain ionomer pellets. In the IR spectrum of the obtained resin, the 1700 cm -1 The peak at 1560 cm originating from the carbonyl group of the carboxylate group decreased. -1 The peak around 1700 cm originating from the carbonyl group of the carboxylic acid (dimer) increased. -1 From the decrease in the peak near the peak, it was confirmed that an ionomer with the desired degree of neutralization had been produced. The physical properties of the obtained ionomer are shown in Tables 5 and 6.

[0125] [Table 5]

[0126] [Table 6]

[0127] <Preparation of Laminated Body Using Ionomer> A substrate was prepared by laminating a 12 μm thick biaxially oriented PET and a 7 μm thick aluminum foil by dry lamination in advance. The aluminum surface of the substrate was extrusion laminated to a thickness of 25 μm using an extrusion lamination device having a 40 mmφ extruder and a T-die with a face length of 300 mm and a lip gap of 0.8 mm, with an air gap of 90 mm, a molding resin temperature of 280 ° C, a cooling roll temperature of 20 ° C, and a line speed of 10 m / min, using ionomer 1 to obtain a laminate. The extrusion lamination conditions and the aluminum adhesive strength and hot tack strength of the obtained laminate are shown in Table 9.

[0128] [Example 2] <Preparation of polymer composition using ionomer> LDPE resin (MFR=5, density=0.918g / cm3) polymerized by autoclave high pressure method with 70% by weight of ionomer 1 3 After uniformly mixing the mixture (Mw / Mn=11, 30% by weight) with a mixer for about 30 seconds, the mixture was kneaded at 170°C with a 30 mmφ single-screw kneading extruder to obtain pellets of polymer composition 1. The MFR of the obtained polymer composition 1 was 6.0 g / 10 min. <Preparation of Laminate Using Polymer Composition Using Ionomer> Extrusion lamination was carried out in the same manner as in Example 1 to obtain a laminate having a thickness of 25 μm, except that the obtained polymer composition 1 was used instead of the ionomer 1. The extrusion lamination conditions and the aluminum adhesive strength and hot tack strength of the obtained laminate are shown in Table 9.

[0129] [Comparative Example 1]: E / MAA-based binary ionomer An ionomer resin (HIMILAN HIM1652, manufactured by Dow Mitsui Polychemicals Co., Ltd.), which is a copolymer of ethylene, methacrylic acid, and zinc methacrylate, and produced by a high-pressure radical process, was used as a reference ionomer. The physical properties are shown in Tables 7 and 8.

[0130] [Table 7]

[0131] [Table 8]

[0132] <Preparation of Laminate Using Polymer Composition Using Ionomer> Extrusion lamination was performed to a thickness of 25 μm in the same manner as in Example 1, except that HIM1652 was used instead of Ionomer 1, to obtain a laminate. The extrusion lamination conditions and the aluminum adhesive strength and hot tack strength of the obtained laminate are shown in Table 9. A graph showing the relationship between temperature and hot tack strength is shown in Figure 3.

[0133] [Table 9]

[0134] <Consideration of the results of the Examples and Comparative Examples> 3, it can be seen that the Examples have extremely high hot tack strength at 120 to 130° C. and are excellent in hot tack properties compared to the Comparative Examples. This is believed to be because the ethylene-based ionomer in the present invention has a substantially linear molecular structure, unlike conventional ionomers. [Industrial Applicability]

[0135] The polymer composition for lamination using the ionomer of the present invention has excellent mechanical properties and adhesion properties compared to ionomers obtained by conventional high-pressure radical polymerization methods, and therefore a laminate using the same has excellent sealing properties and can be usefully used as a packaging material, etc.< / e> < / e>

Claims

1. (X1) A copolymer (P) containing, as essential constituent units, structural units (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms and structural units (B) derived from a monomer having a carboxyl group and / or a dicarboxylic anhydride group, in which at least a portion of the carboxyl groups and / or dicarboxylic anhydride groups are converted to a metal-containing carboxylate containing at least one metal ion selected from Groups 1, 2, or 12 of the periodic table, and the absolute value G of the complex modulus measured with a rotational rheometer is * 100 to 60% by weight of an ionomer having a phase angle δ of 50 degrees to 75 degrees at a pressure of 0.1 MPa; (X2) Ethylene-based copolymer having ethylene as an essential monomer by high-pressure radical polymerization 40-0% by weight and having a melt flow rate of 2.0 to 50 g / 10 min.

2. (X1) A copolymer (P) containing, as essential structural units, a structural unit (A) derived from ethylene and / or an α-olefin having 3 to 20 carbon atoms and a structural unit (B) derived from a monomer having a carboxyl group and / or a dicarboxylic anhydride group, and further containing, as a structural unit, a structural unit (C) other than the structural unit (A) and the structural unit (B) which is a compound having one or more carbon-carbon double bonds in its molecular structure, at least a portion of the carboxyl groups and / or dicarboxylic anhydride groups is converted to a metal-containing carboxylate containing at least one metal ion selected from Groups 1, 2, or 12 of the Periodic Table, and the absolute value G of the complex modulus measured with a rotational rheometer is * 100 to 60% by weight of an ionomer having a phase angle δ of 50 degrees to 75 degrees at a pressure of 0.1 MPa; (X2) Ethylene-based copolymer having ethylene as an essential monomer by high-pressure radical polymerization 40-0% by weight and having a melt flow rate of 2.0 to 50 g / 10 min.

3. The polymer composition for lamination according to claim 2, characterized in that the structural unit (C) in the copolymer (P) is a non-cyclic monomer represented by the following general formula (1) or a cyclic monomer represented by the following general formula (2): [C12] [In general formula (1), T 1 ~T 3 each independently represents a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group having 1 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a hydroxyl group, a hydrocarbon group having 2 to 20 carbon atoms substituted with an alkoxy group having 1 to 20 carbon atoms, a hydrocarbon group having 3 to 20 carbon atoms substituted with an ester group having 2 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an ester group having 2 to 20 carbon atoms, a silyl group having 3 to 20 carbon atoms, a halogen atom, or a cyano group; T 4 is a substituent selected from the group consisting of a hydrocarbon group having 1 to 20 carbon atoms substituted with a hydroxyl group, a hydrocarbon group having 2 to 20 carbon atoms substituted with an alkoxy group having 1 to 20 carbon atoms, a hydrocarbon group having 3 to 20 carbon atoms substituted with an ester group having 2 to 20 carbon atoms, a hydrocarbon group having 1 to 20 carbon atoms substituted with a halogen atom, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an ester group having 2 to 20 carbon atoms, a silyl group having 3 to 20 carbon atoms, a halogen atom, or a cyano group. [C13] [In general formula (2), R 1 ~R 12 may be the same or different and are selected from the group consisting of a hydrogen atom, a halogen atom, and a hydrocarbon group having 1 to 20 carbon atoms; R 9 and R 10 , and R 11 and R 12 may combine together to form a divalent organic group, R 9 Or R 10 And, R 11 Or R 12 may form a ring together. In addition, n represents 0 or a positive integer, and when n is 2 or more, R 5 ~R 8 may be the same or different in each repeating unit.

4. 4. The polymer composition for lamination according to claim 3, wherein the structural unit (C) in the copolymer (P) is a non-cyclic monomer represented by the general formula (1).

5. 4. The polymer composition for lamination according to claim 3, wherein the structural unit (C) in the copolymer (P) is a cyclic monomer represented by the general formula (2).

6. The copolymer (P) 13 6. The polymer composition for lamination according to claim 1, wherein the number of methyl branches calculated by C-NMR is 50 or less per 1,000 carbon atoms.

7. The copolymer (P) 13 6. The polymer composition for lamination according to claim 1, wherein the number of methyl branches calculated by C-NMR is 5 or less per 1,000 carbon atoms.

8. The polymer composition for lamination according to any one of claims 1 to 7, wherein the copolymer (P) contains the structural unit (B) in an amount of 2 to 20 mol % in the copolymer.

9. The polymer composition for lamination according to any one of claims 1 to 8, wherein the structural unit (A) is a structural unit derived from ethylene.

10. The polymer composition for lamination according to any one of claims 1 to 9, characterized in that the copolymer (P) is produced using a transition metal catalyst containing a transition metal of Groups 8 to 11 of the periodic table.

11. 11. The polymer composition for lamination according to claim 10, wherein the transition metal catalyst is a transition metal catalyst comprising a phosphorus sulfonic acid or phosphorus phenol ligand and nickel or palladium.

12. The polymer composition for lamination according to any one of claims 1 to 11, characterized in that the ethylene-based copolymer (X2) obtained by high-pressure radical polymerization is an ethylene homopolymer.

13. A laminate comprising at least an I layer made of a base material layer and an II layer made of a sealant layer, the sealant layer being made of the polymer composition for lamination according to any one of claims 1 to 12.

14. A method for extrusion lamination, comprising extrusion laminating a substrate layer using the polymer composition for lamination according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Method for producing ethylenic ionomer, and the ethylenic ionomer

    JP2016079408A

  • Ionic hydrocarbon polymers

    US3264272A

  • NOVEL METAL COMPLEX, AND METHOD FOR PRODUCING α-OLEFIN POLYMER AND METHOD FOR PRODUCING α-OLEFIN / (METH)ACRYLATE COPOLYMER EACH USING THE METAL COMPLEX

    WO2010050256A1

  • Multi-component ionomer

    WO2020179632A1