Rubber composition for fiber coating and tire

The rubber composition with isoprene rubber, carbon black, and plasticizer, along with silica and resorcin condensates, enhances adhesion to fibers by improving interaction and dispersion, addressing the adhesion issues in tire fiber coatings.

JP7567291B2Active Publication Date: 2024-10-16SUMITOMO RUBBER INDUSTRIES LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020144276
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-28
Publication Date
2024-10-16
Estimated Expiration
2040-08-28

AI Technical Summary

Technical Problem

Existing rubber compositions for fiber coating in tires do not adequately address the issue of adhesion to fibers, particularly under high loads.

Method used

A rubber composition containing isoprene rubber, carbon black with a dibutyl phthalate oil absorption of 100 ml/100 g or more, and a plasticizer, with a specific mass ratio of carbon black to isoprene rubber to plasticizer, enhanced with fillers like silica and resorcin condensates, to improve adhesion.

Benefits of technology

The composition achieves improved adhesion to fibers by promoting interaction and dispersion of carbon black, leading to better reinforcing properties and adhesion forces.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567291000001
    Figure 0007567291000001
  • Figure 0007567291000002
    Figure 0007567291000002
  • Figure 0007567291000003
    Figure 0007567291000003
Patent Text Reader

Abstract

To provide a rubber composition for fiber coating that can achieve improved adhesion to fiber and a tire.SOLUTION: A rubber composition for fiber coating has: a rubber component containing isoprene rubber; a filler containing carbon black with an amount of absorption of dibutyl phthalate of 100 ml / 100 g or more; and a plasticizer. In the filler 100 mass%, the content of the carbon black is 65 mass% or more. [The content of the isoprene rubber>the content of carbon black>the content of the plasticizer] holds.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition for coating fibers and a tire. [Background technology]

[0002] Generally, automobile tires are subjected to a large load, and therefore fibers (fiber cords) are used as reinforcing materials. Conventionally, various studies have been conducted on the adhesion between a rubber composition for covering fibers and fibers (for example, see Patent Document 1), but in recent years, further improvements have been required. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-69199 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a rubber composition for covering fibers, which can solve the above problems and improve adhesion to fibers, and a tire. [Means for solving the problem]

[0005] The present invention relates to a rubber composition for covering fibers, comprising a rubber component containing an isoprene-based rubber, a filler containing carbon black having a dibutyl phthalate oil absorption of 100 ml / 100 g or more, and a plasticizer, wherein the carbon black content is 65 mass % or more in 100 mass % of the filler, and the ratio of the isoprene-based rubber content > the carbon black content > the plasticizer content is satisfied.

[0006] The rubber composition preferably contains a resorcinol condensate and / or a phenol resin.

[0007] Preferably, the filler comprises silica.

[0008] It is preferable that the nitrogen adsorption specific surface area of ​​the carbon black / the dibutyl phthalate oil absorption of the carbon black is less than 0.2.

[0009] The content of the carbon black in 100% by mass of the filler is preferably 85% by mass or more.

[0010] It is preferable that the rubber composition contains sulfur, and the ratio of the sulfur content to the plasticizer content is 0.6 or more.

[0011] The rubber composition preferably contains an organic thiosulfate compound.

[0012] The present invention also relates to a tire having a fiber / rubber composite in which organic fibers are coated with the rubber composition.

[0013] The present invention also relates to a tire having a fiber / rubber composite in which metal fibers are coated with the rubber composition. Effect of the Invention

[0014] The present invention relates to a rubber composition for coating fibers, which contains a rubber component containing an isoprene-based rubber, a filler containing carbon black having a dibutyl phthalate oil absorption of 100 ml / 100 g or more, and a plasticizer, wherein the carbon black content is 65 mass % or more in 100 mass % of the filler, and the ratio of the isoprene-based rubber content > the carbon black content > the plasticizer content is satisfied, and therefore the rubber composition has good adhesion to fibers. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The rubber composition of the present invention contains a rubber component including an isoprene-based rubber, a filler including carbon black having a dibutyl phthalate oil absorption of 100 ml / 100 g or more, and a plasticizer, wherein the content of the carbon black is 65 mass% or more in 100 mass% of the filler, and the content of the isoprene-based rubber > the content of the carbon black > the content of the plasticizer.

[0016] The reason why the above-mentioned effects are obtained with the above-mentioned rubber composition is presumed to be as follows. In the above rubber composition, it is believed that by blending an isoprene-based rubber, carbon black having a DBP oil absorption of 100 ml / 100 g or more, and a plasticizer, and further increasing the proportion of the carbon black in the filler, an interaction between the rubber component and the carbon black is more likely to occur. Furthermore, by making the content of isoprene-based rubber > the content of the carbon black > the content of the plasticizer, the dispersibility of the carbon black during mixing is improved by the plasticizer, and the carbon black is more likely to enter the phase of the isoprene-based rubber, making it easier for an interaction to occur between the rubber component and the carbon black. It is believed that the above-mentioned effects promote the dispersion of the carbon black, thereby improving the reinforcing properties of the isoprene-based rubber and generating a good reaction force at the interface with the fiber, thereby significantly improving adhesion.

[0017] The rubber composition contains a rubber component. Here, the rubber component is a component that contributes to crosslinking, and generally has a weight average molecular weight (Mw) of 10,000 or more.

[0018] The weight average molecular weight of the rubber component is preferably 50,000 or more, more preferably 150,000 or more, and even more preferably 200,000 or more, and is preferably 2,000,000 or less, more preferably 1,500,000 or less, and even more preferably 1,000,000 or less. Within the above ranges, the effect tends to be better obtained.

[0019] In this specification, the weight average molecular weight (Mw) can be determined by converting it into standard polystyrene based on the measured value obtained by gel permeation chromatography (GPC) (GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKGEL SUPERMULTIPORE HZ-M manufactured by Tosoh Corporation).

[0020] The total styrene content in the rubber component is preferably 10% by mass or less, more preferably 5% by mass or less, and further preferably 3% by mass or less, and may be 0% by mass. When it is within the above range, the effect tends to be better obtained.

[0021] Here, the total amount of styrene in the rubber component is the total content of styrene parts contained in the total amount of rubber component (unit: mass%), and can be calculated by Σ(content of each rubber component × amount of styrene in each rubber component / 100). For example, in a case where 100% by mass of rubber component contains 85% by mass of SBR with styrene content: 40% by mass, 5% by mass of SBR with styrene content: 25% by mass, and 10% by mass of BR with styrene content: 0% by mass, the total amount of styrene in the rubber component is 35.25% by mass (=85×40 / 100+5×25 / 100+10×0 / 100).

[0022] The total vinyl content in the rubber component is preferably 10% by mass or less, more preferably 5% by mass or less, and further preferably 3% by mass or less, and may be 0% by mass. When it is within the above range, the effect tends to be better obtained.

[0023] Here, the total vinyl content in the rubber component is the total content of vinyl parts contained in the entire rubber component (unit: mass%) and can be calculated by Σ (content of each rubber component × vinyl content in each rubber component / 100). For example, in a 100% rubber component, when the rubber component contains 85% by mass of SBR with a vinyl content of 30% by mass, 5% by mass of SBR with a vinyl content of 20% by mass, and 10% by mass of BR with a vinyl content of 10% by mass, the total vinyl content in the rubber component is 27.5% by mass (=85×30 / 100+5×20 / 100+10×10 / 100).

[0024] The styrene amount and vinyl amount in each rubber component can be measured by a nuclear magnetic resonance (NMR) method. In addition, in the examples of this specification, the total styrene amount and the total vinyl amount in the rubber component are calculated according to the above-mentioned formula, but they may also be analyzed from the tire using, for example, a pyrolysis gas chromatograph mass spectrometer (Py-GC / MS) or the like.

[0025] The rubber composition contains an isoprene-based rubber as a rubber component. Examples of isoprene-based rubber include natural rubber (NR), isoprene rubber (IR), modified NR, modified NR, and modified IR. Examples of NR include SIR20, RSS♯3, TSR20, and other rubbers that are common in the tire industry. Examples of IR include IR2200 and other rubbers that are common in the tire industry. Examples of modified NR include deproteinized natural rubber (DPNR), high-purity natural rubber (UPNR), and other rubbers. Examples of modified NR include epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), and grafted natural rubber. Examples of modified IR include epoxidized isoprene rubber, hydrogenated isoprene rubber, and grafted isoprene rubber. These may be used alone or in combination of two or more. Among these, NR is preferred.

[0026] In 100% by mass of the rubber component, the content of the isoprene-based rubber is preferably 60% by mass or more, more preferably 80% by mass or more, and further preferably 90% by mass or more, and may be 100% by mass. When it is within the above range, the effect tends to be better obtained.

[0027] Examples of rubber components that can be used other than isoprene-based rubber include diene-based rubbers such as styrene butadiene rubber (SBR), butadiene rubber (BR), acrylonitrile butadiene rubber (NBR), chloroprene rubber (CR), butyl rubber (IIR), and styrene-isoprene-butadiene copolymer rubber (SIBR). These may be used alone or in combination of two or more. Among these, SBR and BR are preferred.

[0028] The SBR is not particularly limited, and for example, emulsion-polymerized styrene-butadiene rubber (E-SBR), solution-polymerized styrene-butadiene rubber (S-SBR), etc. Commercially available products include those from Sumitomo Chemical Co., Ltd., JSR Corporation, Asahi Kasei Corporation, Nippon Zeon Co., Ltd., etc.

[0029] In 100% by mass of the rubber component, the content of SBR is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less. Within the above ranges, the effect tends to be better obtained.

[0030] The BR is not particularly limited, and can be high cis content BR, low cis content BR, BR containing syndiotactic polybutadiene crystals, etc. Commercially available products include those from Ube Industries, Ltd., JSR Corporation, Asahi Kasei Corporation, Zeon Corporation, etc.

[0031] In 100% by mass of the rubber component, the content of BR is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more, and is preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less. Within the above ranges, the effect tends to be better obtained.

[0032] The rubber component may be modified to introduce a functional group that interacts with a filler such as silica. Examples of the functional group include an amino group, an amide group, a silyl group, an alkoxysilyl group, an isocyanate group, an imino group, an imidazole group, a urea group, an ether group, a carbonyl group, an oxycarbonyl group, a mercapto group, a sulfide group, a disulfide group, a sulfonyl group, a sulfinyl group, a thiocarbonyl group, an ammonium group, an imide group, a hydrazo group, an azo group, a diazo group, a carboxyl group, a nitrile group, a pyridyl group, an alkoxy group, a hydroxyl group, an oxy group, and an epoxy group. These functional groups may have a substituent. Among them, an amino group (preferably an amino group in which a hydrogen atom of an amino group is substituted with an alkyl group having 1 to 6 carbon atoms), an alkoxy group (preferably an alkoxy group having 1 to 6 carbon atoms), and an alkoxysilyl group (preferably an alkoxysilyl group having 1 to 6 carbon atoms) are preferred.

[0033] Specific examples of compounds (modifiers) having the above-mentioned functional groups include 2-dimethylaminoethyltrimethoxysilane, 3-dimethylaminopropyltrimethoxysilane, 2-dimethylaminoethyltriethoxysilane, 3-dimethylaminopropyltriethoxysilane, 2-diethylaminoethyltrimethoxysilane, 3-diethylaminopropyltrimethoxysilane, 2-diethylaminoethyltriethoxysilane, 3-diethylaminopropyltriethoxysilane, and the like.

[0034] The rubber composition contains carbon black having a dibutyl phthalate (DBP) oil absorption of 100 ml / 100 g or more as a filler. Examples of the carbon black include N134, N110, N220, N234, N339, N330, N351, and N550. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Corporation, Lion Corporation, Shinnikka Carbon Co., Ltd., Columbia Carbon Co., Ltd., and the like. These may be used alone or in combination of two or more kinds.

[0035] The DBP oil absorption of the carbon black is preferably 100 ml / 100 g or more, and more preferably 120 ml / 100 g or more. 2 / g or more, more preferably 130m 2 / g or more, more preferably 140m 2 / g or more, and preferably 180m 2 / g or less, more preferably 160m 2 / g or less, more preferably 150m 2 Within the above range, there is a tendency for the effect to be better obtained. The DBP oil absorption of carbon black can be measured in accordance with JIS-K6217-4:2001.

[0036] The nitrogen adsorption specific surface area (N2SA) of the carbon black is preferably 5 m 2 / g or more, more preferably 15m 2 / g or more, more preferably 20m 2 / g or more, and preferably 85m 2 / g or less, more preferably 65m 2 / g or less, more preferably 45m 2 / g or less, particularly preferably 30m 2 Within the above range, there is a tendency for the effect to be better obtained. The N2SA of carbon black is a value measured in accordance with JIS K6217-2:2001.

[0037] The N2SA of the carbon black / DBP oil absorption of the carbon black is preferably less than 0.8, more preferably less than 0.5, and even more preferably less than 0.2, and is preferably 0.1 or more. When it is within the above range, the effect tends to be better.

[0038] The amount of the carbon black is preferably 15 parts by mass or more, more preferably 35 parts by mass or more, even more preferably 45 parts by mass or more, and particularly preferably 50 parts by mass or more, and is preferably 80 parts by mass or less, more preferably 70 parts by mass or less, and even more preferably 60 parts by mass or less, based on 100 parts by mass of the rubber component. When the amount is within the above range, the effect tends to be better obtained.

[0039] From the viewpoint of adhesion to fibers, etc., it is preferable that the rubber composition satisfy the relationship: the content (unit: parts by mass) of the carbon black>the N2SA of the carbon black.

[0040] The carbon black content / N2SA of the carbon black is preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more, and is preferably 4.0 or less, more preferably 3.0 or less, and even more preferably 2.5 or less. Within the above ranges, the effect tends to be better.

[0041] The content of the carbon black in 100% by mass of the filler is 65% by mass or more, preferably 75% by mass or more, more preferably 85% by mass or more, and even more preferably 90% by mass or more, and is preferably 98% by mass or less, more preferably 95% by mass or less. When it is within the above range, the effect tends to be better.

[0042] Fillers that can be used other than the carbon black include those commonly used in the tire industry, such as silica, calcium compounds, aluminum hydroxide, talc, mica, magnesium oxide, and magnesium sulfate. Carbon blacks other than the carbon blacks mentioned above (carbon blacks with DBP oil absorption of less than 100 ml / 100 g) can also be used. These may be used alone or in combination of two or more. Among these, silica and calcium compounds are preferred.

[0043] Examples of silica include dry silica (anhydrous silicic acid) and wet silica (hydrated silicic acid), but wet silica is preferred because it has a large number of silanol groups. Commercially available products include those from EVONIK, Tosoh Silica Co., Ltd., Solvay Japan Co., Ltd., Tokuyama Co., Ltd., etc. These may be used alone or in combination of two or more.

[0044] The cetyltrimethylammonium bromide (CTAB) specific surface area of ​​the silica is preferably 180 m 2 / g, more preferably less than 170m 2 / g or less, and preferably 100m 2 / g or more, preferably 130m 2 / g or more, more preferably 150m 2 Within the above range, there is a tendency for the effect to be better obtained. The CTAB specific surface area of ​​silica is measured in accordance with ASTM D3765-92.

[0045] The content of silica is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.

[0046] The calcium compound is a compound containing calcium, and examples thereof include inorganic salts such as calcium oxide, calcium hydroxide, and calcium carbide; and oxoacid salts such as calcium carbonate, calcium nitrate, and calcium sulfate. The oxoacid salts also include fatty acid salts such as calcium acetate and calcium stearate. In addition, examples of compounds containing calcium compounds include eggshells (main component: calcium carbonate) and WB16 (a mixture of fatty acid calcium, fatty acid amide, and fatty acid amide ester) manufactured by Struktol. These may be used alone or in combination of two or more. Among these, oxoacid salts are preferred, and calcium carbonate is more preferred.

[0047] In the rubber composition, the content of the calcium compound is, calculated as calcium element, preferably 3 parts by mass or more, more preferably 6 parts by mass or more, and even more preferably 8 parts by mass or more, and is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 12 parts by mass or less, per 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.

[0048] The amount of the filler is preferably 30 parts by mass or more, more preferably 45 parts by mass or more, and even more preferably 55 parts by mass or more, and is preferably 80 parts by mass or less, more preferably 65 parts by mass or less, and even more preferably 60 parts by mass or less, based on 100 parts by mass of the rubber component. When the amount is within the above range, the effect tends to be better obtained.

[0049] The rubber composition preferably contains a silane coupling agent. The silane coupling agent is not particularly limited, and examples thereof include bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl)trisulfide, bis(4-trimethoxysilylbutyl)trisulfide, bis(3-triethoxysilylpropyl)disulfide, bis(2-triethoxysilylethyl)disulfide, bis(4-triethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, bis(3-trimethoxysilylpropyl)disulfide, bis(2-trimethoxysilylethyl)disulfide, bis(4-trimethoxysilylbutyl)disulfide, 3-trimethoxysilylpropyl, mercapto-based compounds such as 3-mercaptopropyltrimethoxysilane and 2-mercaptoethyltriethoxysilane; vinyl-based compounds such as vinyltriethoxysilane and vinyltrimethoxysilane; amino-based compounds such as 3-aminopropyltriethoxysilane and 3-aminopropyltrimethoxysilane; glycidoxy-based compounds such as γ-glycidoxypropyltriethoxysilane and γ-glycidoxypropyltrimethoxysilane; nitro-based compounds such as 3-nitropropyltrimethoxysilane and 3-nitropropyltriethoxysilane; and chloro-based compounds such as 3-chloropropyltrimethoxysilane and 3-chloropropyltriethoxysilane. As commercially available products, for example, products from Degussa, Momentive, Shin-Etsu Silicone Co., Ltd., Tokyo Chemical Industry Co., Ltd., Azumax Co., Ltd., Dow Corning Toray Co., Ltd., etc. can be used. These may be used alone or in combination of two or more kinds.

[0050] The content of silane coupling agent is preferably 3 parts by mass or more, more preferably 6 parts by mass or more, even more preferably 8 parts by mass or more, and is preferably 15 parts by mass or less, more preferably 12 parts by mass or less, even more preferably 10 parts by mass or less, based on 100 parts by mass of silica.When it is within the above range, the effect tends to be better obtained.

[0051] The rubber composition preferably contains a resin. As the resin, a resorcinol condensate (resorcinol resin) or a phenolic resin can be suitably used. These may be used alone or in combination of two or more kinds.

[0052] As the resorcinol condensate, for example, a compound (resin) represented by the following formula can be used. [ka] (In the formula, n is an integer of 1 or more.)

[0053] The resorcinol condensate may be a modified resorcinol condensate. As the modified resorcinol condensate, for example, a compound (resin) represented by the following formula can be used. [ka] (In the formula, n is an integer of 1 or more, and R is an alkyl group.)

[0054] As commercially available resorcinol condensates, products from Taoka Chemical Co., Ltd., Indospec, etc. can be used.

[0055] The phenolic resin is obtained by reacting phenol with an aldehyde such as formaldehyde in the presence of an acid or alkali catalyst.

[0056] The phenolic resin may be modified with cashew oil, tall oil, rosin, etc. The modified phenolic resin is preferably a cashew oil modified phenolic resin. For example, the compound (resin) represented by the following formula can be used as the cashew oil modified phenolic resin. [ka] (In the formula, p is an integer of 1 to 9, and preferably 5 to 6.)

[0057] As commercially available phenolic resins, products from Sumitomo Bakelite Co., Ltd. and the like can be used.

[0058] The amount of the resin is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and is preferably 15 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 8 parts by mass or less, based on 100 parts by mass of the rubber component. When the amount is within the above range, the effect tends to be better obtained.

[0059] In the rubber composition, the resin content / silica content is preferably 0.2 or more, more preferably 0.5 or more, even more preferably 0.8 or more, and is preferably 1.8 or less, more preferably 1.5 or less, even more preferably 1.2 or less, and particularly preferably 1.0 or less. Within the above ranges, the effect tends to be better obtained. In this relationship, the resin content and the silica content are the contents (unit: parts by mass) relative to 100 parts by mass of the rubber component.

[0060] In the rubber composition, the resin content / carbon black content having a DBP oil absorption of 100 ml / 100 g or more is preferably 0.1 or more, and preferably 1.0 or less, more preferably 0.8 or less, and further preferably 0.5 or less. Within the above ranges, the effect tends to be better. In this regard, the resin content and the carbon black content are the contents (unit: parts by mass) relative to 100 parts by mass of the rubber component.

[0061] The rubber composition preferably contains an organic thiosulfate compound. As the organic thiosulfate compound, for example, a compound represented by the following formula or a hydrate thereof can be used. MO3S-S-(CH2) q -S-SO3M (In the formula, q represents an integer of 3 to 10. M may be the same or different and represents lithium, potassium, sodium, magnesium, calcium, barium, zinc, nickel, or cobalt.)

[0062] q is preferably at least 4, more preferably at least 5, and is preferably at most 8, more preferably at most 6. Within the above ranges, there is a tendency for better effects to be obtained.

[0063] M is preferably lithium, potassium or sodium, more preferably sodium.

[0064] From the viewpoint of adhesiveness to fibers, etc., the organic thiosulfate compound is preferably a derivative derived from sodium thiosulfate, and more preferably 1,6-hexamethylene-sodium dithiosulfate dihydrate.

[0065] The content of the organic thiosulfate compound is preferably 1 part by mass or more, more preferably 1.2 parts by mass or more, and even more preferably 1.5 parts by mass or more, and is preferably 4 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.

[0066] The rubber composition preferably contains an organic acid cobalt. Examples of organic acid cobalt include cobalt stearate, cobalt naphthenate, cobalt neodecanoate, boron 3 cobalt neodecanoate, and cobalt abithienate. Commercially available products include those from Dai-Nippon Ink and Chemicals, Inc. These may be used alone or in combination of two or more. Among these, cobalt stearate is preferred.

[0067] The content of the organic cobalt acid is preferably 0.1 parts by mass or more, and preferably 1.2 parts by mass or less, more preferably 0.8 parts by mass or less, and further preferably 0.5 parts by mass or less, calculated as elemental cobalt, per 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.

[0068] The rubber composition preferably contains a methylene donor. Examples of methylene donors include hexamethylenetetramine (HMT), hexamethoxymethylolmelamine (HMMM), and hexamethylolmelamine pentamethylether (HMMPME). Commercially available products include those from Taoka Chemical Co., Ltd. These may be used alone or in combination of two or more. Among these, HMT and HMMPME are preferred, and HMMPME is more preferred.

[0069] The content of the methylene donor is preferably 0.5 parts by mass or more, more preferably 0.8 parts by mass or more, even more preferably 1.2 parts by mass or more, and particularly preferably 1.5 parts by mass or more, and is preferably 4 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.

[0070] The rubber composition contains a plasticizer. As the plasticizer, for example, oil (including the oil content in oil-extended rubber), liquid polymer, ester-based plasticizer, etc. can be used. These may be used alone or in combination of two or more.

[0071] The content of the plasticizer is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and is preferably 30 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.

[0072] In the above rubber composition, the following relationship is satisfied: content of isoprene-based rubber>content of carbon black having a DBP oil absorption of 100 ml / 100 g or more>content of plasticizer.

[0073] The ratio of the isoprene rubber content to the carbon black content is preferably 1.5 or more, more preferably 1.8 or more, and even more preferably 2.0 or more, and is preferably 4.0 or less, more preferably 3.0 or less, and even more preferably 2.5 or less. Within the above ranges, the effect tends to be better.

[0074] The carbon black content / plasticizer content is preferably 3 or more, more preferably 6 or more, and even more preferably 8 or more, and is preferably 15 or less, more preferably 12 or less, and even more preferably 10 or less. Within the above ranges, the effect tends to be better obtained.

[0075] In these relationships, the isoprene-based rubber content is the content (unit: mass %) in 100% by mass of the rubber component, and the carbon black content and the plasticizer content are the contents (unit: mass parts) relative to 100 parts by mass of the rubber component.

[0076] From the viewpoint of adhesiveness to fibers, the plasticizer is preferably oil. Examples of the oil include process oil, vegetable oil, and mixtures thereof. Examples of the process oil include paraffin-based process oil, aromatic process oil, and naphthenic process oil. Examples of the vegetable oil include castor oil, cottonseed oil, linseed oil, rapeseed oil, soybean oil, palm oil, coconut oil, peanut oil, rosin, pine oil, pine tar, tall oil, corn oil, rice oil, safflower oil, sesame oil, olive oil, sunflower oil, palm kernel oil, camellia oil, jojoba oil, macadamia nut oil, and tung oil. Examples of commercially available products include products from Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., JXTG Nippon Oil & Energy Corporation, Orisoi Co., Ltd., H&R Co., Ltd., Toyokuni Oil Mill Co., Ltd., Showa Shell Sekiyu K.K., Fuji Kosan Co., Ltd., and the like. These may be used alone or in combination of two or more.

[0077] The content of the oil is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and is preferably 30 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better obtained.

[0078] The rubber composition preferably contains sulfur. In the rubber composition after vulcanization, most of the sulfur is bonded to the rubber component. Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, insoluble sulfur, highly dispersible sulfur, soluble sulfur, etc., which are generally used as crosslinking agents in the rubber industry. Commercially available products include those from Tsurumi Chemical Industry Co., Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemical Industry Co., Ltd., Flexis Corporation, Nippon Kanzuri Kogyo Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds. Sulfur is also contained in organic thiosulfate compounds, dialkyldithiophosphate compounds, sulfide-based silane coupling agents, thiazole-based vulcanization accelerators, thiuram-based vulcanization accelerators, sulfenamide-based vulcanization accelerators, sulfenimide-based vulcanization accelerators, and the like.

[0079] The amount of sulfur is preferably 1.5 parts by mass or more, more preferably 3.5 parts by mass or more, even more preferably 4.5 parts by mass or more, particularly preferably 5.2 parts by mass or more, and is preferably 8.5 parts by mass or less, more preferably 7.5 parts by mass or less, and even more preferably 6.5 parts by mass or less, based on 100 parts by mass of the rubber component. When the amount is within the above range, the effect tends to be better obtained. In this specification, the sulfur content includes not only the sulfur used as a crosslinking agent but also the sulfur content in sulfur-containing compounds such as organic thiosulfate compounds. The sulfur content may be calculated from the amount of chemicals used, or may be analyzed from the tire by, for example, an oxygen combustion flask method in accordance with JIS-K6233:2016.

[0080] The sulfur content / plasticizer content is preferably 0.2 or more, more preferably 0.6 or more, even more preferably 0.9 or more, particularly preferably 1.0 or more, and is preferably 2.5 or less, more preferably 2.0 or less, even more preferably 1.5 or less. Within the above ranges, the effect tends to be better. In this relationship, the sulfur content and the plasticizer content are the contents (unit: parts by mass) relative to 100 parts by mass of the rubber component.

[0081] The rubber composition may contain a vulcanization accelerator. Examples of the vulcanization accelerator include thiazole-based vulcanization accelerators such as 2-mercaptobenzothiazole and di-2-benzothiazolyl disulfide; thiuram-based vulcanization accelerators such as tetramethylthiuram disulfide (TMTD) and tetrakis(2-ethylhexyl)thiuram disulfide (TOT-N); sulfenamide-based vulcanization accelerators such as N-cyclohexyl-2-benzothiazylsulfenamide (CBS), N-tert-butyl-2-benzothiazolylsulfenamide (TBBS), N-oxyethylene-2-benzothiazolesulfenamide and N,N'-diisopropyl-2-benzothiazolesulfenamide; guanidine-based vulcanization accelerators such as diphenylguanidine, di-orthotolylguanidine and orthotolylbiguanidine; and sulfenimide-based vulcanization accelerators such as N-tert-butyl-2-benzothiazolylsulfenimide (TBSI). As commercially available products, products of Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Industry Co., Ltd., etc. can be used. These may be used alone or in combination of two or more. Among them, sulfenamide-based vulcanization accelerators and sulfenimide-based vulcanization accelerators are preferred, sulfenimide-based vulcanization accelerators are more preferred, and N-tert-butyl-2-benzothiazolylsulfenimide is even more preferred.

[0082] The content of the vulcanization accelerator is preferably 0.8 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 1.2 parts by mass or more, and is preferably 6 parts by mass or less, more preferably 4 parts by mass or less, and even more preferably 3 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better.

[0083] The rubber composition may contain a wax. The wax is not particularly limited, and examples thereof include petroleum waxes such as paraffin wax and microcrystalline wax; natural waxes such as vegetable wax and animal wax; and synthetic waxes such as polymers of ethylene, propylene, etc. Commercially available products include those from Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., Seiko Chemical Co., Ltd., etc. These may be used alone or in combination of two or more kinds.

[0084] The amount of the wax is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better obtained.

[0085] The rubber composition may contain stearic acid. As the stearic acid, a conventionally known one can be used, and as a commercially available product, a product from NOF Corp., Kao Corp., Fujifilm Wako Pure Chemical Corp., Chiba Fatty Acid Corp., etc. can be used. These may be used alone or in combination of two or more kinds.

[0086] The content of stearic acid is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 6 parts by mass or less, based on 100 parts by mass of the rubber component. When the content is within the above range, the effect tends to be better obtained.

[0087] The rubber composition may contain zinc oxide. As the zinc oxide, a conventionally known one can be used, and as a commercially available product, it is possible to use products from Mitsui Mining & Smelting Co., Ltd., Toho Zinc Co., Ltd., Hakusui Tech Co., Ltd., Seido Chemical Industry Co., Ltd., Sakai Chemical Industry Co., Ltd., etc. These may be used alone or in combination of two or more kinds.

[0088] The amount of zinc oxide per 100 parts by mass of the rubber component is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and is preferably 12 parts by mass or less, more preferably 10 parts by mass or less, and more preferably 8 parts by mass or less. Within the above ranges, the effect tends to be better obtained.

[0089] The rubber composition may contain an antioxidant. Examples of the antioxidant include naphthylamine-based antioxidants such as phenyl-α-naphthylamine; diphenylamine-based antioxidants such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine, and N,N'-di-2-naphthyl-p-phenylenediamine. Examples of the antioxidant include p-phenylenediamine antioxidants such as quinolinone; quinoline antioxidants such as polymers of 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis, tris, and polyphenol antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Commercially available products include those from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., and Flexis Co., Ltd. These may be used alone or in combination of two or more.

[0090] The content of the antioxidant is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and is preferably 12 parts by mass or less, more preferably 10 parts by mass or less, and even more preferably 8 parts by mass or less, based on 100 parts by mass of the rubber component. Within the above ranges, the effect tends to be better.

[0091] In addition to the above components, the rubber composition may further contain additives commonly used in the tire industry, such as organic peroxides, etc. The content of these additives is preferably 0.1 to 200 parts by mass per 100 parts by mass of the rubber component.

[0092] The rubber composition can be produced, for example, by kneading the above-mentioned components using a rubber kneading device such as an open roll or a Banbury mixer, and then vulcanizing the mixture.

[0093] As for the kneading conditions, in the base kneading step in which additives other than the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 100 to 180°C, preferably 120 to 170°C. In the finish kneading step in which the vulcanizing agent and the vulcanization accelerator are kneaded, the kneading temperature is usually 120°C or lower, preferably 85 to 110°C. Furthermore, the composition kneaded with the vulcanizing agent and the vulcanization accelerator is usually subjected to a vulcanization treatment such as press vulcanization. The vulcanization temperature is usually 140 to 190°C, preferably 150 to 185°C. The vulcanization time is usually 5 to 15 minutes.

[0094] The rubber composition is used for covering (topping) fibers (fiber cords). Examples of the fibers include organic fibers such as polyester fibers, nylon fibers, rayon fibers, polyethylene naphthalate fibers, and aramid fibers; and metal fibers such as steel fibers, stainless steel fibers, nickel fibers, titanium fibers, copper fibers, and aluminum fibers.

[0095] Examples of the fiber / rubber composite in which the fiber is covered with the rubber composition include carcasses, breakers, bands, and the like.

[0096] The carcass is a component disposed inside the tread and radially outside the inner liner, and specifically, is a component shown in FIG. 1 of JP-A-2004-67027 and the like.

[0097] The breaker is a component disposed inside the tread and radially outside the carcass, and specifically is a component shown in FIG. 3 of JP-A No. 2003-94918, FIG. 1 of JP-A No. 2004-67027, and FIGS. 1 to 4 of JP-A No. 4-356205.

[0098] The band is a member provided on the outer side of the breaker in the tire radial direction so as to be in contact with the breaker, and is, for example, a member shown in FIG. 1 of JP 2009-138043 A.

[0099] The tire of the present invention is produced by a conventional method using the above rubber composition. That is, the rubber composition is extruded into a desired shape while still unvulcanized, and molded together with other tire components in a tire building machine by a normal method to form an unvulcanized tire. The unvulcanized tire is then heated and pressurized in a vulcanizer to obtain a tire.

[0100] The above tires (pneumatic tires, etc.) can be used for passenger car tires; truck and bus tires; motorcycle tires; high-performance tires; winter tires such as studless tires; run-flat tires with side reinforcing layers; tires with sound-absorbing material that have a sound-absorbing material such as sponge in the tire cavity; tires with sealing material that have a sealant inside or in the tire cavity that can seal in the event of a puncture; and tires with electronic components that have electronic components such as sensors and wireless tags inside or in the tire cavity, and are suitable for passenger car tires and truck and bus tires.

[0101] The size of the tire is not particularly limited, and can be appropriately selected, for example, from a tire width in the range of 100 to 400 mm, an aspect ratio in the range of 25 to 85%, and a rim diameter in the range of 10 to 25 inches. Specific examples include 105 / 50R16, 115 / 50R17, 125 / 55R20, 135 / 45R21, 145 / 45R21, 155 / 45R18, 165 / 45R22, 175 / 45R23, 185 / 60R20, 195 / 55R14, 205 / 40R16, 215 / 40R16, 225 / 40R17, 235 / 40R17, 245 / 40R16, 255 / 40R17, 265 / 40R17, 275 / 35R18, 285 / 30R19, and 295 / 45R20.

[0102] It is preferable that the tire outer diameter Dt and the tire section width Wt of the tire satisfy the following relational expression.

number

[0103] Specific examples of tires that can satisfy the above formula include 145 / 60R18, 145 / 60R19, 155 / 55R18, 155 / 55R19, 155 / 70R17, 155 / 70R19, 165 / 55R20, 165 / 55R21, 165 / 60R19, 165 / 65R19, 165 / 70R18, 175 / 55R19, 175 / 55R20, 175 / 55R22, 175 / 60R18, 185 / 55R19, 185 / 60R20, 195 / 50R20, 195 / 55R20, and the like.

[0104] A tire satisfying the above formula is preferably applied to a pneumatic tire for a passenger vehicle, because a pneumatic tire for a passenger vehicle satisfying the above formula tends to be more suitable for solving the problem of the present invention. EXAMPLES

[0105] The present invention will be specifically described based on examples, but the present invention is not limited to these examples.

[0106] The various chemicals used in the examples and comparative examples will be described below.

[0107] (Rubber component) Natural rubber: TSR20 SBR: JSR1502 manufactured by JSR Corporation (styrene content: 24% by mass, vinyl content: 16% by mass) BR: BR150B manufactured by Ube Industries, Ltd. (cis content: 97% by mass, vinyl content: 1% by mass)

[0108] (Chemicals other than rubber components) Carbon black 1: Asahi #50U (N2SA:23m) manufactured by Asahi Carbon Co., Ltd.2 / g, DBP: 63ml / 100g) Carbon black 2: Diablack N330 (N2SA:79m) manufactured by Mitsubishi Chemical Corporation 2 / g, DBP: 105ml / 100g) Carbon black 3: Nitelon #SH SRF-HS (N2SA:24m) manufactured by Nippon Steel Carbon Co., Ltd. 2 / g, DBP: 140ml / 100g) Calcium carbonate: Takehara Chemical Industry Co., Ltd.'s Tankal #200 (calcium element content: approx. 40% by mass) Silica: Ultrasil VN3 (CTAB: 165m) manufactured by Evonik Degussa 2 / g) Oil: A / O Mix manufactured by Sankyo Yuka Kogyo Co., Ltd. Wax: Ozoace 0355 manufactured by Nippon Seiro Co., Ltd. Organic thiosulfate compound: Flexis DURALINK HTS (sodium 1,6-hexamethylene dithiosulfate dihydrate) Resin 1: Sumikanol 620 (modified resorcinol condensate, softening point: 100°C) manufactured by Taoka Chemical Co., Ltd. Resin 2: PR12686 (cashew oil modified phenolic resin) manufactured by Sumitomo Bakelite Co., Ltd. Stearic acid: NOF Corporation's "Tsubaki" stearic acid Cobalt stearate: Cost-F (cobalt content: 9.5% by mass) manufactured by Dainippon Ink and Chemicals, Inc. Zinc oxide: Zinc oxide No. 1 manufactured by Mitsui Mining & Smelting Co., Ltd. Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Industry Co., Ltd. Methylene donor 1: Sumikanol 507AP (partial condensate of hexamethylol melamine pentamethyl ether (HMMPME), containing 30% by mass of silica) manufactured by Taoka Chemical Co., Ltd. Methylene donor 2: Noccela H (hexamethylenetetramine (HMT)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 1: Noccela NS (N-tert-butyl-2-benzothiazolyl sulfenamide) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Vulcanization accelerator 2: Santocure TBSI (N-tert-butyl-2-benzothiazolyl sulfenimide) manufactured by Flexis Co., Ltd.

[0109] Examples and Comparative Examples According to the composition shown in Table 1, materials other than sulfur and vulcanization accelerator were kneaded for 5 minutes at 150°C using a 1.7L Banbury mixer manufactured by Kobe Steel, Ltd. to obtain a kneaded product. Next, sulfur and vulcanization accelerator were added to the kneaded product obtained, and the mixture was kneaded for 5 minutes at 80°C using an open roll to obtain a sheet-shaped unvulcanized rubber composition. The resulting unvulcanized rubber composition was used to sandwich both sides of the polyester fiber arrangement, and press-vulcanized at 150° C. for 12 minutes to obtain a test sample 1 (polyester fiber / rubber composite). Also, both sides of an array of steel fibers were sandwiched using the unvulcanized rubber composition obtained, and press-vulcanized at 150° C. for 12 minutes to obtain a test sample 2 (steel fiber / rubber composite). The obtained test samples 1 and 2 were used to carry out the following evaluations, and the results are shown in Table 1. In Table 1, oil corresponds to the plasticizer.

[0110] (Adhesion 1: Adhesion to polyester fiber) Using the test sample 1, the stress when the cord (polyester fiber) was pulled out was measured according to a method in accordance with JIS L 1017:2002. The maximum value of the measured stress was expressed as an index, with the value of Comparative Example 5 being 100. A larger index indicates better adhesion to the polyester fiber.

[0111] (Adhesion 2: Adhesion to steel fibers) Using test sample 2, the stress when the cord (steel fiber) was pulled out was measured according to a method in accordance with JIS G 3510: 1992. The maximum value of the measured stress was expressed as an index, with Comparative Example 8 being set at 100. A larger index indicates better adhesion to the steel fiber.

[0112] [Table 1]

[0113] As can be seen from Table 1, the Examples had better adhesion to the intended fibers than the Comparative Examples.

Claims

1. The rubber composition contains a rubber component containing an isoprene-based rubber, a filler containing carbon black having a dibutyl phthalate oil absorption of 100 ml / 100 g or more, and a plasticizer, The content of the carbon black is 65% by mass or more in 100% by mass of the filler, the content of the isoprene-based rubber > the content of the carbon black > the content of the plasticizer, the nitrogen adsorption specific surface area of ​​the carbon black / the dibutyl phthalate oil absorption of the carbon black is less than 0.2; the plasticizer is at least one selected from the group consisting of oils and liquid polymers, The rubber composition for fiber coating has a plasticizer content of 1 part by mass or more and 30 parts by mass or less per 100 parts by mass of the rubber component.

2. A rubber composition comprising a rubber component containing isoprene-based rubber, a filler containing carbon black having a dibutyl phthalate oil absorption of 100 ml / 100 g or more, and a plasticizer; The content of the carbon black is 65% by mass or more in 100% by mass of the filler, the content of the isoprene-based rubber > the content of the carbon black > the content of the plasticizer, the ratio of the carbon black content to the plasticizer content is 8 to 15, The resin content / silica content is 0.8 or more, the plasticizer is at least one selected from the group consisting of oils and liquid polymers, The rubber composition for fiber coating has a plasticizer content of 1 part by mass or more and 30 parts by mass or less per 100 parts by mass of the rubber component.

3. 3. The rubber composition for fiber coating according to claim 1, further comprising a resorcinol condensate and / or a phenolic resin.

4. 4. The rubber composition for fiber coating according to claim 1, wherein the filler contains silica.

5. 3. The rubber composition for fiber coating according to claim 2, wherein the nitrogen adsorption specific surface area of ​​said carbon black / the dibutyl phthalate oil absorption of said carbon black is less than 0.

2.

6. 6. The rubber composition for fiber coating according to claim 1, wherein the content of said carbon black is 85% by mass or more based on 100% by mass of said filler.

7. Contains sulfur, 7. The rubber composition for fiber coating according to claim 1, wherein the ratio of the sulfur content to the plasticizer content is 0.6 or more.

8. The rubber composition for fiber coating according to any one of claims 1 to 7, which contains an organic thiosulfate compound.

9. A tire having a fiber / rubber composite in which organic fibers are coated with the rubber composition according to any one of claims 1 to 8.

10. A tire having a fiber / rubber composite in which metal fibers are coated with the rubber composition according to any one of claims 1 to 8.

Citation Information

Patent Citations

  • Rubber composition for coating fixed cord and tire having carcass and / or belt using the same

    JP2008069199A

  • Rubber composition for coating steel cord and tire having belt or breaker obtained by covering steel cord with the same

    JP2008156418A

  • Rubber composition for coating tire cord

    JP2009007549A

  • Rubber composition for tire cord covering, breaker edge strip, breaker cushion or cord-adjacent strip, and pneumatic tire

    JP2013122038A

  • Rubber composition for steel cord cover, breaker edge strip, breaker cushion or strip adjacent to cord, and pneumatic tire

    JP2014080475A