Composition for forming resin layer, vinyl chloride resin laminate sheet and method for producing same, and laminate

A resin layer formed with a specific resin and organometallic compound composition addresses plasticizer migration and enhances durability in vinyl chloride resin laminates, ensuring effective suppression of plasticizer migration and improved heat and humidity resistance.

JP7567777B2Active Publication Date: 2024-10-16ZEON CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021508895
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-26
Filing Date
2020-03-03
Publication Date
2024-10-16
Estimated Expiration
2040-03-03

AI Technical Summary

Technical Problem

The migration of plasticizer from vinyl chloride resin molded sheets to foamed polyurethane in laminates used for automobile interior materials leads to deterioration of the vinyl chloride resin, and existing solutions do not adequately address the issues of plasticizer migration and durability under high temperature and humidity conditions.

Method used

A resin layer forming composition containing a resin with an SP value greater than 14 (cal/cm³)¹/² and a degree of polymerization of 300 or more, along with an organometallic compound, is applied to the vinyl chloride resin molded sheet to form a resin layer that suppresses plasticizer migration and enhances heat and humidity resistance.

Benefits of technology

The resin layer effectively prevents plasticizer migration and improves the durability of the vinyl chloride resin laminate sheet under high temperature and humidity conditions, maintaining its integrity and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567777000001
    Figure 0007567777000001
  • Figure 0007567777000002
    Figure 0007567777000002
  • Figure 0007567777000003
    Figure 0007567777000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide a composition for forming a resin layer, from which a resin layer that can prevent the migration of a plasticizer from a vinyl chloride resin molded sheet satisfactorily and has excellent wet heat resistance can be formed. The composition for forming a resin layer according to the present invention comprises a resin A and an organic metal compound, the composition being characterized in that the SP value of the resin A is 14 (cal / cm3)1 / 2 or more and the degree of polymerization of the resin A is 300 or more.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin layer-forming composition, a vinyl chloride resin laminate sheet and a method for producing the same, and a laminate. [Background technology]

[0002] Polyvinyl chloride resins are generally used in a variety of applications due to their excellent properties such as cold resistance, heat resistance, and oil resistance. Specifically, for example, automobile interior parts such as automobile instrument panels have conventionally been formed using automobile interior materials such as a skin made of a vinyl chloride resin molded product (hereinafter, sometimes referred to as a "vinyl chloride resin molded sheet") obtained by molding a vinyl chloride resin composition into a sheet shape, or a laminate made by lining a foam such as polyurethane foam on the skin made of the vinyl chloride resin molded sheet.

[0003] As a material for the vinyl chloride resin molded sheet, a vinyl chloride resin composition containing a vinyl chloride resin and a plasticizer is used (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2011-173974 A [Patent Document 2] JP 2012-7026 A Summary of the Invention [Problem to be solved by the invention]

[0005] Here, when a laminate formed by backing a foam such as polyurethane foam on a skin made of a vinyl chloride resin molded sheet is used as an automobile interior material, the plasticizer contained in the vinyl chloride resin molded sheet migrates to the foam, and the amount of plasticizer in the vinyl chloride resin molded sheet decreases, which may cause deterioration such as a decrease in flexibility of the vinyl chloride resin molded sheet (i.e., the skin). Therefore, in the laminate used as the above-mentioned automobile interior material, it is required to effectively suppress the migration of the plasticizer from the vinyl chloride resin molded sheet to the foam.

[0006] Therefore, the present inventors have found that such problems can be solved by using a vinyl chloride resin laminate sheet in which a resin layer having a resin with a SP value in a predetermined range as a main component is disposed on at least one side in the thickness direction of a vinyl chloride resin molded sheet containing a plasticizer. Specifically, the present inventors have found that when a laminate is produced by lining a polyurethane foam molded body on the side on which the resin layer is disposed in the vinyl chloride resin laminate sheet (i.e., the vinyl chloride resin molded sheet and the polyurethane foam molded body are bonded via the resin layer), migration of the plasticizer from the vinyl chloride resin molded sheet can be effectively suppressed.

[0007] However, after further investigation, the present inventors found that when a laminate was produced using the above-mentioned vinyl chloride resin laminate sheet, a resin layer having as its main component a resin whose SP value falls within the specified range as described above had room for improvement in durability (i.e., moist heat resistance) under high humidity and high temperature conditions (e.g., humidity of 80% RH or higher, temperature of 80°C or higher).

[0008] Therefore, an object of the present invention is to provide a resin layer-forming composition that can effectively suppress migration of a plasticizer from a polyvinyl chloride resin molded sheet and can form a resin layer that has excellent resistance to moist heat. Another object of the present invention is to provide a polyvinyl chloride resin laminate sheet which is capable of effectively suppressing migration of a plasticizer from a polyvinyl chloride resin molded sheet and which has a resin layer with excellent wet heat resistance, and a method for producing the same. It is yet another object of the present invention to provide a laminate which is capable of effectively preventing migration of a plasticizer from a polyvinyl chloride resin molded sheet and which has excellent resistance to moist heat. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above problems, and have found that by using a resin layer-forming composition containing a resin having a SP value and a degree of polymerization equal to or greater than a predetermined value, and an organometallic compound, migration of a plasticizer from a vinyl chloride resin molded sheet can be effectively suppressed, and a resin layer having excellent wet heat resistance can be formed, thereby completing the present invention.

[0010] That is, the present invention has an object to advantageously solve the above-mentioned problems, and the resin layer forming composition of the present invention is a resin layer forming composition containing a resin A and an organometallic compound, wherein the SP value of the resin A is 14 (cal / cm 3 ) 1 / 2 and the degree of polymerization of the resin A is not less than 300. In this way, a resin layer-forming composition containing a resin having an SP value and a degree of polymerization not less than a predetermined value and an organometallic compound can satisfactorily suppress migration of a plasticizer from a polyvinyl chloride resin molded sheet and can form a resin layer having excellent moist heat resistance.

[0011] Here, the SP value means the solubility parameter. The SP value can be calculated using the method introduced in Hansen Solubility Parameters A User's Handbook, 2nd Ed (CRC Press). The SP value of an organic compound can also be estimated from the molecular structure of the organic compound. Specifically, it can be calculated using simulation software that can calculate the SP value from the SMILE formula (e.g., "HSPiP" (http: / / www.hansen-solubility.com)). This simulation software calculates the SP value based on the theory described in Hansen SOLUBILITY PARAMETERS A User's Handbook Second Edition, Charles M. Hansen.

[0012] The degree of polymerization refers to the number of monomer units contained in the polymer that constitutes the resin. For example, when polyvinyl alcohol is used as resin A, the degree of polymerization of polyvinyl alcohol as resin A can be determined as an average degree of polymerization measured according to the method described in JIS K6726.

[0013] Here, the resin layer-forming composition of the present invention preferably has a content of the organometallic compound of 3.00 parts by mass or more and 10.00 parts by mass or less relative to 100 parts by mass of the resin A. In this way, if the content of the organometallic compound is within the above-mentioned predetermined range, the moist heat resistance of the formed resin layer can be further improved, and the storage stability of the resin layer-forming composition can be improved.

[0014] In the resin layer-forming composition of the present invention, the organometallic compound preferably contains an organotitanium compound. When the organometallic compound contains an organotitanium compound, the moist heat resistance of the resin layer to be formed can be further improved.

[0015] Furthermore, the present invention aims to advantageously solve the above problems, and the vinyl chloride resin laminate sheet of the present invention is a vinyl chloride resin laminate sheet having a vinyl chloride resin molded sheet containing a vinyl chloride resin and a plasticizer, and a resin layer L arranged on at least one side in the thickness direction of the vinyl chloride resin molded sheet, characterized in that the resin layer L is formed using any of the above-mentioned resin layer forming compositions. In this way, a vinyl chloride resin laminate sheet formed by forming a resin layer L on at least one side in the thickness direction of a vinyl chloride resin molded sheet containing a vinyl chloride resin and a plasticizer using any of the above-mentioned resin layer forming compositions can effectively suppress the migration of the plasticizer from the vinyl chloride resin molded sheet, and has excellent moist heat resistance of the resin layer.

[0016] The vinyl chloride resin laminate sheet of the present invention is preferably used for the surface of an automobile instrument panel. By using the vinyl chloride resin laminate sheet of the present invention as the surface of an automobile instrument panel, the migration of plasticizer from the vinyl chloride resin molded sheet can be effectively suppressed, and deterioration of the surface can be prevented.

[0017] Furthermore, the method for producing a vinyl chloride resin laminate sheet of the present invention is characterized by including a coating step of coating any one of the above-mentioned resin layer forming compositions on at least one side in the thickness direction of a vinyl chloride resin molded sheet containing a vinyl chloride resin and a plasticizer, and a resin layer forming step of drying the coated resin layer forming composition to form a resin layer L. In this way, the vinyl chloride resin laminate sheet produced by coating any one of the above-mentioned resin layer forming compositions on at least one side in the thickness direction of a vinyl chloride resin molded sheet containing a vinyl chloride resin and a plasticizer, and then drying the coated resin layer forming composition to form a resin layer L, can satisfactorily suppress the migration of the plasticizer from the vinyl chloride resin molded sheet, and has excellent moist heat resistance of the resin layer.

[0018] Furthermore, the present invention aims to advantageously solve the above problems, and the laminate of the present invention is a laminate having a polyurethane foam molded body and any of the vinyl chloride resin laminate sheets described above, characterized in that the resin layer L is disposed between the polyurethane foam molded body and the vinyl chloride resin molded sheet. In this way, a laminate having a polyurethane foam molded body and any of the vinyl chloride resin laminate sheets described above, in which the resin layer L is disposed between the polyurethane foam molded body and the vinyl chloride resin molded sheet, can effectively suppress migration of plasticizer from the vinyl chloride resin molded sheet, and has excellent moist heat resistance. Effect of the Invention

[0019] According to the present invention, it is possible to provide a resin layer-forming composition that can effectively suppress migration of a plasticizer from a vinyl chloride resin molded sheet and can form a resin layer that has excellent moist heat resistance. Furthermore, according to the present invention, it is possible to provide a polyvinyl chloride resin laminate sheet which can effectively suppress migration of a plasticizer from a polyvinyl chloride resin molded sheet and has a resin layer with excellent moist heat resistance, and a method for producing the same. Furthermore, according to the present invention, it is possible to provide a laminate which can effectively inhibit migration of plasticizer from a polyvinyl chloride resin molded sheet and has excellent resistance to moist heat. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] Hereinafter, an embodiment of the present invention will be described in detail. Here, the resin layer forming composition of the present invention can be used, for example, in the production of the vinyl chloride resin laminate sheet of the present invention. Moreover, the vinyl chloride resin laminate sheet of the present invention has a resin layer L formed using the resin layer forming composition of the present invention. Furthermore, the vinyl chloride resin laminate sheet of the present invention can be used, for example, in the production of the laminate of the present invention. And, the vinyl chloride resin laminate sheet of the present invention can be suitably used as an automobile interior material, such as the skin of an automobile interior part such as an automobile instrument panel. Furthermore, the vinyl chloride resin laminate sheet of the present invention can be produced by the method for producing a vinyl chloride resin laminate sheet of the present invention.

[0021] (Composition for forming resin layer) The resin layer forming composition of the present invention is characterized by containing a resin A having a SP value and a degree of polymerization equal to or greater than a predetermined value, and an organometallic compound. By using the resin layer forming composition of the present invention, migration of a plasticizer from a vinyl chloride resin molded sheet can be effectively suppressed, and a resin layer having excellent wet heat resistance can be formed. The resin layer-forming composition of the present invention may optionally contain other components in addition to the resin A and the organometallic compound. The resin layer-forming composition of the present invention is usually prepared by dispersing or dissolving the above-mentioned resin A, the organometallic compound, and other components in a known solvent.

[0022] <Resin A> Resin A functions as a matrix resin (base material) in the resin layer L formed using the resin layer-forming composition, and is a component that can effectively inhibit migration of the plasticizer from the vinyl chloride resin molded sheet. The content of the resin A in the resin layer-forming composition can be adjusted as desired within a range in which the desired effects of the present invention can be obtained.

[0023] Here, the SP value of resin A is 14 (cal / cm 3 ) 1 / 2 It must be 15(cal / cm 3 ) 1 / 2It is preferable that the calorie content is 16 (cal / cm 3 ) 1 / 2 It is more preferable that the SP value of resin A is 14 (cal / cm 3 ) 1 / 2 If the SP value of resin A is 30 (cal / cm 2 ), the migration of the plasticizer from the polyvinyl chloride resin molded sheet can be effectively suppressed. 3 ) 1 / 2 It is preferable that the calorie content is 25 (cal / cm 3 ) 1 / 2 More preferably, it is 22 (cal / cm 3 ) 1 / 2 More preferably, it is 20 (cal / cm 3 ) 1 / 2 It is particularly preferable that the SP value of resin A is 30 (cal / cm 3 ) 1 / 2 If it is equal to or less than this, the flexibility of the resin layer L can be increased.

[0024] The degree of polymerization of resin A must be 300 or more, preferably 320 or more, more preferably 350 or more, even more preferably 380 or more, even more preferably 400 or more, and preferably 1000 or less, more preferably 800 or less, and even more preferably 600 or less. If the degree of polymerization of resin A is the above lower limit or more, the moist heat resistance of the resin layer formed can be improved. On the other hand, if the degree of polymerization of resin A is the above upper limit or less, the resulting resin layer-forming composition has excellent handleability during coating.

[0025] Further, the molecular weight of the resin A is not particularly limited, but the weight average molecular weight (Mw) in terms of polystyrene measured by gel permeation chromatography (GPC) using THF as a solvent is preferably 21000 or more, more preferably 22000 or more, even more preferably 24000 or more, and preferably 70000 or less, more preferably 56000 or less, and even more preferably 42000 or less. If the weight average molecular weight of the resin A is the above lower limit or more, the moist heat resistance of the formed resin layer can be further improved. On the other hand, if the weight average molecular weight of the resin A is the above upper limit or less, the obtained resin layer forming composition has excellent handling properties during coating.

[0026] The above-mentioned resin A is, for example, polyvinyl alcohol (also called a completely saponified product of polyvinyl acetate or a partially saponified product of polyvinyl acetate. The degree of saponification of polyvinyl acetate is 60% or more and the SP value is 14 (cal / cm 3 ) 1 / 2 or more), ethylene-vinyl alcohol copolymer (also called EVA resin), polyacrylamide (SP value = 19.2 (cal / cm 3 ) 1 / 2 (The units of SP value in the rest of this specification are the same), polymethacrylamide (SP value = 19.2), poly N-vinylformamide (SP value = 17.2), water-soluble starch (SP value = 23.5), hydroxyethyl cellulose (SP value = 19.3), hydroxypropyl cellulose (SP value = 18.0), methyl cellulose (SP value = 17.4), ethyl cellulose (SP value = 16.2), chitosan (SP value = 20.4), etc. can be used. Among them, it is preferable to use a resin having a hydroxyl group (-OH group) as the resin A, and it is particularly preferable to use polyvinyl alcohol. If a resin having a hydroxyl group (-OH group) is used as the resin A, the polymers constituting the resin A can be well crosslinked with each other by an organometallic compound described later, and the moist heat resistance of the formed resin layer can be further improved. Furthermore, if polyvinyl alcohol is used as the resin A, the formed resin layer can more effectively suppress the migration of the plasticizer from the polyvinyl chloride resin molded sheet. Note that the "hydroxyl group (-OH group)" in the above does not include, for example, the -OH structure in the carboxyl group (-COOH) of acrylic resins such as polyacrylic acid and polymethacrylic acid.

[0027] The degree of saponification from polyvinyl acetate in polyvinyl alcohol can be 60% or more, preferably 61% or more, more preferably 62% or more, even more preferably 63% or more, even more preferably 65% ​​or more, and can be 100%, preferably less than 100%, preferably 90% or less, more preferably 80% or less, and even more preferably 70% or less. If the degree of saponification from polyvinyl acetate in polyvinyl alcohol is the above lower limit or more, the formed resin layer can more effectively suppress the migration of plasticizer from the vinyl chloride resin molded sheet. On the other hand, if the degree of saponification from polyvinyl acetate in polyvinyl alcohol is the above upper limit or less, the flexibility of the formed resin layer can be increased. The degree of saponification of polyvinyl alcohol from polyvinyl acetate can be measured in accordance with JIS K6726 (Testing method for polyvinyl alcohol).

[0028] Specific examples of polyvinyl alcohol that can be used as resin A include a completely saponified product from polyvinyl acetate (SP value = 23.4), a product with a degree of saponification from polyvinyl acetate of 90% (SP value = 19.1), a product with a degree of saponification from polyvinyl acetate of 80% (SP value = 17.5), a product with a degree of saponification from polyvinyl acetate of 65% (SP value = 16.4), etc. Among these, it is preferable to use a product with a degree of saponification from polyvinyl acetate of 65% from the viewpoints of further suppressing migration of the plasticizer from the vinyl chloride resin molded sheet and increasing the adhesion of the resin layer L to the vinyl chloride resin molded sheet.

[0029] <Organometallic compounds> The organometallic compound functions as a crosslinking agent that crosslinks the polymers constituting the resin A described above, and is a component that can enhance the moist heat resistance of the resin layer that is formed.

[0030] The organometallic compound is not particularly limited as long as it can satisfactorily crosslink the polymers constituting the resin A, and for example, an organotitanium compound, an organozirconium compound, etc. can be used. Among them, it is preferable to use an organotitanium compound from the viewpoint of further improving the moist heat resistance of the resin layer to be formed.

[0031] As the organic titanium compound, for example, it is preferable to use a titanium chelate compound. Here, the titanium chelate compound contains a chelating agent capable of coordinating with titanium atoms. For example, the titanium chelate compound may contain a chelating agent such as hydroxycarboxylic acid and / or its salt, such as lactic acid, a triethanolamine, such as triethanolamine, or 2-(2-aminoethylamino)ethanol. In particular, from the viewpoint of further enhancing the moist heat resistance of the resin layer to be formed, it is preferable to use a titanium chelate compound containing a hydroxycarboxylic acid and / or a salt thereof as a chelating agent, it is more preferable to use a titanium chelate compound containing lactic acid and / or a salt thereof as a chelating agent, it is even more preferable to use a titanium chelate compound containing a salt of lactic acid as a chelating agent, and it is particularly preferable to use a titanium chelate compound containing an ammonium salt of lactic acid as a chelating agent.

[0032] Specific examples of titanium chelate compounds containing a hydroxycarboxylic acid and / or its salt as a chelating agent include titanium lactate (ritical formula: Ti(OH)2[OCH(CH3)COOH]2; also called dihydroxybis(lactate)titanium), titanium lactate ammonium salt (ritical formula: Ti(OH)2[OCH(CH3)COO - ]2(NH4 + ) 2; sometimes called dihydroxybis(ammonium lactate) titanium. ) etc. A specific example of a titanium chelate compound containing a trialcoholamine as a chelating agent is titanium triethanolamine (rational formula: Ti(Oi-C3H7)2(C6H 14 O3N)2; also known as titanium diisopropoxybis(triethanolaminate). ) and the like. A specific example of a titanium chelate compound containing 2-(2-aminoethylamino)ethanol as a chelating agent is titanium aminoethylaminoethanolate (rational formula: (i-C3H7O)Ti(OC2H4NHC2H4NH2)3).

[0033] In addition, from the viewpoint of further enhancing the wet heat resistance of the resin layer to be formed, the titanium chelate compound may be the above-mentioned titanium lactate (rational formula: Ti(OH)2[OCH(CH3)COOH]2), titanium lactate ammonium salt (rational formula: Ti(OH)2[OCH(CH3)COO - ]2(NH4 +It is preferable to use titanium chelate compounds having a hydroxyl group directly bonded to the titanium atom, such as 2).

[0034] Here, as the organometallic compound, commercially available products can also be used. For example, examples of organic titanium compounds that can be used include "TC-300" (titanium lactate ammonium salt), "TC-310" (titanium lactate), "TC-315" (titanium lactate), "TC-335" (titanium lactate), "TC-400" (titanium triethanolamine), and "TC-510" (titanium aminoethylaminoethanolate), all manufactured by Matsumoto Fine Chemical Co., Ltd. As the organic zirconium compound, "ZC-126" (zirconium chloride compound) manufactured by Matsumoto Fine Chemical Co., Ltd. can also be used.

[0035] The content of the organometallic compound in the resin layer forming composition is preferably 3.00 parts by mass or more, more preferably 3.50 parts by mass or more, and even more preferably 4.00 parts by mass or more, and preferably 10.00 parts by mass or less, more preferably 8.00 parts by mass or less, and even more preferably 6.00 parts by mass or less, relative to 100 parts by mass of resin A. If the content of the organometallic compound in the resin layer forming composition is the above lower limit or more, the moist heat resistance of the formed resin layer can be further improved. On the other hand, if the content of the organometallic compound in the resin layer forming composition is the above upper limit or less, the pH of the resin layer forming composition does not increase excessively, and the components in the resin layer forming composition are suppressed from precipitating, and the storage stability of the resin layer forming composition can be improved.

[0036] <Other ingredients> The resin layer-forming composition of the present invention may optionally contain other components in addition to the above-mentioned resin A and organometallic compound. Examples of such other components that can be used include a binder, a plasticizer for the resin layer, and a dispersant.

[0037] <<Binder>> The resin layer forming composition of the present invention may optionally contain a binder. By containing a binder in the resin layer forming composition, the adhesiveness of the formed resin layer to the vinyl chloride resin molded sheet can be increased. Note that the binder is a component different from the above-mentioned resin A.

[0038] As the binder, it is preferable to use a urethane-based binder or an acrylic ester-based binder, and it is more preferable to use a urethane-based binder. If at least one of a urethane-based binder and an acrylic ester-based binder is used as the binder, the adhesiveness of the formed resin layer to the vinyl chloride resin molded sheet can be further increased.

[0039] Here, the urethane-based binder is a polyurethane obtained by reacting isocyanates with polyols, etc. As the urethane-based binder, polyester-based polyurethane obtained by using polyester polyol as the polyol, polycarbonate-based polyurethane obtained by using polycarbonate polyol as the polyol, polyether-based polyurethane obtained by using polyether polyol as the polyol, polycarbonate polyester-based polyurethane obtained by using a mixture of polycarbonate polyol and polyester polyol as the polyol, polyester polyether-based polyurethane obtained by using a mixture of polyester polyol and polyether polyol as the polyol, etc. can be used. From the viewpoint of further enhancing the adhesion of the resin layer to the vinyl chloride resin molded sheet, it is preferable to use a polyester-based polyurethane, a polycarbonate-based polyurethane, or a polycarbonate-polyester-based polyurethane as the urethane-based binder, it is more preferable to use a polyester-based polyurethane or a polycarbonate-based polyurethane, and it is even more preferable to use a polyester-based polyurethane.

[0040] The polyurethane that can be used as the urethane-based binder may be either a yellowing polyurethane obtained by using an aromatic polyisocyanate as the isocyanate, or a non-yellowing polyurethane obtained by using an aliphatic polyisocyanate as the isocyanate. From the viewpoint of further enhancing the adhesion of the resin layer to the vinyl chloride resin molded sheet, however, a yellowing polyurethane obtained by using an aromatic polyisocyanate as the isocyanate is more preferable.

[0041] As the urethane-based binder, commercially available products can be used. As commercially available urethane-based binders, "Toatan S" (polycarbonate polyester polyurethane) manufactured by Tohpe Corporation, "Superflex (registered trademark) 460" (non-yellowing type polycarbonate polyurethane) manufactured by Daiichi Kogyo Seiyaku Co., Ltd., and "Superflex (registered trademark) 740" (yellowing type polyester polyurethane) manufactured by Daiichi Kogyo Seiyaku Co., Ltd. can be suitably used.

[0042] As the acrylic ester binder, a known acrylic ester polymer capable of functioning as a binder can be used. Here, the acrylic ester polymer is a polymer containing a structural unit derived from a (meth)acrylic acid ester monomer. The acrylic ester polymer is obtained by polymerizing a monomer composition containing a (meth)acrylic acid ester monomer and, optionally, an acidic group-containing monomer, an α,β-unsaturated nitrile monomer, and other monomers. As each of the above monomers, a known monomer can be used.

[0043] The content of the binder in the resin layer forming composition is, in terms of dry mass, preferably 2.5 parts by mass or more, more preferably 3.3 parts by mass or more, even more preferably 4.0 parts by mass or more, even more preferably 5.0 parts by mass or more, and preferably 25.0 parts by mass or less, more preferably 20.0 parts by mass or less, even more preferably 15.0 parts by mass or less, particularly preferably 10.0 parts by mass or less, and most preferably 7.5 parts by mass or less, relative to 100 parts by mass of resin A. If the content of the binder in the resin layer forming composition is the above lower limit or more, the adhesiveness of the formed resin layer to the vinyl chloride resin molded sheet can be further increased. On the other hand, if the content of the binder in the resin layer forming composition is the above upper limit or less, the formed resin layer can further suppress the migration of the plasticizer from the vinyl chloride resin molded sheet.

[0044] <<Plasticizer for resin layer>> The resin layer forming composition of the present invention may optionally contain a plasticizer for the resin layer. By containing the resin layer forming composition plasticizer for the resin layer, the resin layer formed can exhibit excellent flexibility. Therefore, the flexibility of the vinyl chloride resin laminate sheet having the resin layer can be increased. Here, when polyvinyl alcohol is used as the resin A, the plasticizer for the resin layer can impart particularly excellent flexibility to the resin layer formed.

[0045] As the plasticizer for the resin layer, it is preferable to use a diol compound having 1 to 4 carbon atoms, such as methylene glycol, ethylene glycol, n-propylene glycol, or n-butylene glycol; or a polyalkylene oxide modified with an alkyl terminal, such as methyl polyglycol or ethyl polyglycol; and it is more preferable to use a polyalkylene oxide modified with an alkyl terminal. If the above-mentioned compound is used as the plasticizer for the resin layer, the flexibility of the formed resin layer can be further increased.

[0046] From the viewpoint of further increasing the flexibility of the resin layer to be formed, the terminal alkyl group in the terminally alkyl-modified polyalkylene oxide is preferably an alkyl group having 1 to 4 carbon atoms, more preferably a methyl group and / or an ethyl group, and even more preferably a methyl group. The terminally alkyl-modified polyalkylene oxide may be either alkyl-modified at both ends or alkyl-modified at one end, but is preferably alkyl-modified at one end.

[0047] From the viewpoint of further increasing the flexibility of the resin layer to be formed, the polyalkylene oxide used in the preparation of the terminally alkylated polyalkylene oxide is preferably polyethylene oxide and / or polypropylene oxide, more preferably polyethylene oxide. The number average degree of polymerization of the polyalkylene oxide is preferably 2 or more, preferably 20 or less, more preferably 10 or less.

[0048] Therefore, it is particularly preferable to use, as the terminally alkyl-modified polyalkylene oxide, methyl polyglycol (also called "polyethylene glycol monomethyl ether"), which is a polyethylene oxide modified with a methyl terminal.

[0049] The content of the plasticizer for the resin layer in the composition for forming the resin layer is preferably 2.5 parts by mass or more, more preferably 3.3 parts by mass or more, more preferably 3.5 parts by mass or more, even more preferably 4.0 parts by mass or more, even more preferably 5.0 parts by mass or more, and preferably 20.0 parts by mass or less, more preferably 15.0 parts by mass or less, even more preferably 10.0 parts by mass or less, even more preferably 8.0 parts by mass or less, and even more preferably 7.0 parts by mass or less, relative to 100 parts by mass of resin A. If the content of the plasticizer for the resin layer in the composition for forming the resin layer is the above lower limit or more, the flexibility of the formed resin layer can be further increased. On the other hand, if the content of the plasticizer for the resin layer in the composition for forming the resin layer is the above upper limit or less, the formed resin layer can further suppress the migration of the plasticizer from the vinyl chloride resin molded sheet.

[0050] <<Dispersant>> The resin layer forming composition of the present invention may optionally contain a dispersant. By containing a dispersant in the resin layer forming composition, any component such as a binder can be well dispersed in the resin layer forming composition. Therefore, the storage stability of the resin layer forming composition can be improved.

[0051] The dispersant is not particularly limited, and a known dispersant can be used, but a surfactant can be preferably used as the dispersant. Examples of the surfactant include nonionic surfactants such as polyoxyalkylene alkyl ethers; anionic surfactants such as sodium dodecylbenzenesulfonate; cationic surfactants such as dodecylammonium chloride; and the like. Among them, nonionic surfactants are more preferred. The content of the dispersant in the resin layer forming composition can be adjusted arbitrarily within the range in which the desired effect of the present invention can be obtained.

[0052] <Solvent> The resin layer forming composition is usually prepared by dissolving or dispersing the above-mentioned resin A, organometallic compound, and other components in a known solvent. As the solvent, known solvents such as water, formic acid, acetic acid, methanol, ethanol, n-propyl alcohol, isopropyl alcohol, diacetone alcohol, dimethyl ether, and diethyl ether can be used depending on the properties of the resin A and the organometallic compound. These solvents may be used alone or in combination. The content of the solvent in the resin layer-forming composition can be appropriately adjusted within a range in which the desired effects of the present invention can be obtained.

[0053] <Method for preparing composition for forming resin layer> The method for preparing the resin layer-forming composition of the present invention is not particularly limited as long as it can provide a composition containing the above-mentioned resin A and an organometallic compound. For example, the resin layer-forming composition can be prepared by adding the resin A, the organometallic compound, and any other components to the above-mentioned solvent and mixing them by a method such as stirring. When adding and mixing each of the above-mentioned components, the solvent may be appropriately heated or cooled depending on the properties of each component to adjust the temperature to a level at which each component can be well dissolved or dispersed. For example, resin A and, if necessary, a plasticizer and dispersant for the resin layer are added to a solvent, and the mixture is stirred and mixed while heating at a temperature of preferably 40°C or higher and 50°C or lower until the components such as resin A are dissolved or dispersed in the solvent, and then the mixture is cooled preferably to 35°C or lower, more preferably to room temperature (23°C), after which an organometallic compound and, if necessary, a binder (e.g., a urethane-based binder) are further added and mixed to prepare a composition for forming a resin layer.

[0054] (Vinyl chloride resin laminated sheet) The vinyl chloride resin laminate sheet of the present invention is characterized in that it has a vinyl chloride resin molded sheet containing a vinyl chloride resin and a plasticizer, and a resin layer L arranged on at least one side in the thickness direction of the vinyl chloride resin molded sheet, and the resin layer L is formed using the above-mentioned resin layer forming composition.

[0055] Furthermore, in the vinyl chloride resin laminate sheet of the present invention, a resin layer L formed using the above-mentioned resin layer forming composition is disposed on at least one side in the thickness direction of the vinyl chloride resin molded sheet, so that migration of plasticizer from the vinyl chloride resin molded sheet can be effectively suppressed and the resin layer has excellent moist heat resistance.

[0056] Therefore, the polyvinyl chloride resin laminate sheet of the present invention is suitably used as an automobile interior member, specifically, for example, as the surface of an automobile interior part such as an automobile instrument panel or door trim, and is particularly suitably used for the surface of an automobile instrument panel.

[0057] <Vinyl chloride resin molded sheet> A vinyl chloride resin molded sheet containing a vinyl chloride resin and a plasticizer can be obtained by molding a vinyl chloride resin composition containing a vinyl chloride resin and a plasticizer into a sheet.

[0058] <<Vinyl chloride resin composition>> The vinyl chloride resin composition contains a vinyl chloride resin and a plasticizer, and may further contain various additives, if desired.

[0059] [Vinyl chloride resin] Here, the vinyl chloride resin contained in the vinyl chloride resin composition may contain, for example, one or more kinds of vinyl chloride resin particles, and may further contain, optionally, one or more kinds of vinyl chloride resin microparticles. Among them, the vinyl chloride resin preferably contains at least vinyl chloride resin particles, and more preferably contains vinyl chloride resin particles and vinyl chloride resin microparticles. In this specification, "resin particles" refers to particles having a particle diameter of 30 μm or more, and "resin fine particles" refers to particles having a particle diameter of less than 30 μm. Vinyl chloride resin particles usually function as a matrix resin (base material), and vinyl chloride resin fine particles usually function as a dusting agent (powder flow improver). Vinyl chloride resin particles are preferably produced by a suspension polymerization method, and vinyl chloride resin fine particles are preferably produced by an emulsion polymerization method. Moreover, the vinyl chloride resin can be produced by any of the conventionally known production methods, such as suspension polymerization, emulsion polymerization, solution polymerization, and bulk polymerization.

[0060] -composition- Examples of vinyl chloride resins include homopolymers consisting of vinyl chloride monomer units, as well as vinyl chloride copolymers containing preferably 50% by mass or more, more preferably 70% by mass or more, of vinyl chloride monomer units. Specific examples of monomers (comonomers) that can be copolymerized with vinyl chloride monomers and that can form vinyl chloride copolymers include olefins such as ethylene and propylene; halogenated olefins such as allyl chloride, vinylidene chloride, vinyl fluoride, and trifluoroethylene chloride; vinyl esters of carboxylic acids such as vinyl acetate and vinyl propionate; vinyl ethers such as isobutyl vinyl ether and cetyl vinyl ether; allyl ethers such as allyl-3-chloro-2-oxypropyl ether and allyl glycidyl ether; acrylic acid, maleic acid, itaconic acid, acrylic acid- Examples of the comonomer include unsaturated carboxylic acids such as 2-hydroxyethyl, methyl methacrylate, monomethyl maleate, diethyl maleate, and maleic anhydride, esters thereof, and anhydrides thereof; unsaturated nitriles such as acrylonitrile and methacrylonitrile; acrylamide, N-methylolacrylamide, acrylamido-2-methylpropanesulfonic acid, and (meth)acrylamidopropyltrimethylammonium chloride; allylamine and its derivatives such as allylamine benzoate and diallyldimethylammonium chloride. The above-mentioned monomers are only a part of the comonomers, and as the comonomer, various monomers exemplified in "Polyvinyl Chloride" edited by Kinki Chemical Association Vinyl Division, Nikkan Kogyo Shimbun (1988), pp. 75-104, can be used. Only one of these comonomers may be used, or two or more of them may be used. The vinyl chloride resin also includes resins obtained by graft polymerization of (1) vinyl chloride or (2) vinyl chloride with the above-mentioned comonomer onto resins such as ethylene-vinyl acetate copolymer, ethylene-methyl methacrylate copolymer, ethylene-ethyl acrylate copolymer, and chlorinated polyethylene. In this specification, "(meth)acrylic" means acrylic and / or methacrylic.

[0061] -SP value- The SP value of the polymer used as polyvinyl chloride resin is 8 (cal / cm 3 ) 1 / 2 It is preferable that the calorie content is 9 (cal / cm 3 ) 1 / 2 More preferably, it is 11 (cal / cm 3 ) 1 / 2 It is preferable that the calorie content is 10 (cal / cm 3 ) 1 / 2 If the SP value of the polymer used as the vinyl chloride resin is within the above-mentioned range, migration of the plasticizer from the vinyl chloride resin molded sheet can be more effectively suppressed.

[0062] [Plasticizer] If the vinyl chloride resin composition does not contain a plasticizer, it is not possible to satisfactorily obtain a vinyl chloride resin molded sheet using the vinyl chloride resin composition.

[0063] The "plasticizer" used in the vinyl chloride resin composition is a component different from the "plasticizer for resin layer" that can be used in the above-mentioned composition for forming a resin layer (i.e., that can be contained in the resin layer L described below). In this specification, the term "plasticizer" does not refer to the "plasticizer for resin layer" that can be contained in the resin layer L, but refers to the "plasticizer" used in the vinyl chloride resin composition, i.e., the "plasticizer" contained in the vinyl chloride resin molded sheet.

[0064] -Content- Here, the content of the plasticizer is preferably 70 parts by mass or more, more preferably 80 parts by mass or more, even more preferably 92 parts by mass or more, even more preferably 97 parts by mass or more, and preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 100 parts by mass or less, relative to 100 parts by mass of the vinyl chloride resin. If the content of the plasticizer is equal to or more than the lower limit, the vinyl chloride resin composition is given excellent flexibility, and for example, it is easy to process into a vinyl chloride resin molded sheet, and the obtained vinyl chloride resin molded sheet can be given good tensile elongation at low temperatures. Also, if the content of the plasticizer is equal to or less than the upper limit, the stickiness of the surface of the obtained vinyl chloride resin molded sheet can be further suppressed, and the surface slipperiness can be further increased.

[0065] -kinds- Specific examples of the plasticizer include the following primary plasticizers and secondary plasticizers. The so-called primary plasticizers include trimethyl trimellitate, triethyl trimellitate, tri-n-propyl trimellitate, tri-n-butyl trimellitate, tri-n-pentyl trimellitate, tri-n-hexyl trimellitate, tri-n-heptyl trimellitate, tri-n-octyl trimellitate, di-n-octyl-mono-n-decyl trimellitate, mono-n-octyl-di-n-decyl trimellitate, tri-n-nonyl trimellitate, tri-n-decyl trimellitate, tri-n-undecyl trimellitate, tri-n-dodecyl trimellitate, tri-n-pentyl trimellitate, tri-n-hexyl trimellitate, tri-n-heptyl trimellitate, tri-n-octyl-di-n-decyl trimellitate, tri-n-nonyl trimellitate, tri-n-decyl trimellitate, tri-n-undecyl trimellitate, tri-n-dodecyl trimellitate, tri-n-pentyl trimellitate, tri-n-hex ... Linear trimellitic acid esters in which the alkyl group constituting the ester is linear, such as n-tridecyl, tri-n-tetradecyl trimellitate, tri-n-pentadecyl trimellitate, tri-n-hexadecyl trimellitate, tri-n-heptadecyl trimellitate, tri-n-stearyl trimellitate, and tri-n-alkyl trimellitate (wherein the carbon numbers of the alkyl groups in the tri-n-alkyl trimellitate may be different from each other in one molecule) (note that these trimellitic acid esters may be composed of a single compound or a mixture); Tri-i-propyl trimellitate, Tri-i-butyl trimellitate, Tri-i-pentyl trimellitate, Tri-i-hexyl trimellitate, Tri-i-heptyl trimellitate, Tri-i-octyl trimellitate, Tri-(2-ethylhexyl) trimellitate, Tri-i-nonyl trimellitate, Tri-i-decyl trimellitate, Tri-i-undecyl trimellitate, Tri-i-dodecyl trimellitate, Tri-i-tridecyl trimellitate, Tri-i-tetradecyl trimellitate, branched trimellitic acid esters in which the alkyl group constituting the ester is branched, such as tri-i-pentadecyl trimellitate, tri-i-hexadecyl trimellitate, tri-i-heptadecyl trimellitate, tri-i-octadecyl trimellitate, and trialkyl trimellitate (wherein the carbon numbers of the alkyl groups in the trialkyl trimellitate may be different from each other in one molecule); (Note that these trimellitic acid esters may be composed of a single compound or a mixture.); Tetramethyl pyromellitic acid, tetraethyl pyromellitic acid, tetra-n-propyl pyromellitic acid, tetra-n-butyl pyromellitic acid, tetra-n-pentyl pyromellitic acid, tetra-n-hexyl pyromellitic acid, tetra-n-heptyl pyromellitic acid, tetra-n-octyl pyromellitic acid, tetra-n-nonyl pyromellitic acid, tetra-n-decyl pyromellitic acid, tetra-n-undecyl pyromellitic acid, tetra-n-dodecyl pyromellitic acid, tetra-n-tridecyl pyromellitic acid, tetra-n-tetradecyl pyromellitic acid, pyromellitic acid Linear pyromellitic acid esters in which the alkyl group constituting the ester is linear, such as tetra-n-pentadecyl romellitic acid, tetra-n-hexadecyl pyromellitic acid, tetra-n-heptadecyl pyromellitic acid, tetra-n-stearyl pyromellitic acid, and tetra-n-alkyl pyromellitic acid esters (wherein the number of carbon atoms of the alkyl groups in the pyromellitic acid tetra-n-alkyl esters may be different from each other in one molecule) (note that these pyromellitic acid esters may be composed of a single compound or a mixture); Tetra-i-propyl pyromellitic acid, tetra-i-butyl pyromellitic acid, tetra-i-pentyl pyromellitic acid, tetra-i-hexyl pyromellitic acid, tetra-i-heptyl pyromellitic acid, tetra-i-octyl pyromellitic acid, tetra-(2-ethylhexyl) pyromellitic acid, tetra-i-nonyl pyromellitic acid, tetra-i-decyl pyromellitic acid, tetra-i-undecyl pyromellitic acid, tetra-i-dodecyl pyromellitic acid, tetra-i-tridecyl pyromellitic acid, tetra-i-tetradecyl pyromellitic acid, Branched pyromellitic acid esters in which the alkyl group constituting the ester is branched, such as tetra-i-pentadecyl romellitic acid, tetra-i-hexadecyl pyromellitic acid, tetra-i-heptadecyl pyromellitic acid, tetra-i-octadecyl pyromellitic acid, and pyromellitic acid tetraalkyl esters (wherein the carbon numbers of the alkyl groups in the pyromellitic acid tetraalkyl esters may be different from each other in one molecule) (note that these pyromellitic acid esters may be composed of a single compound or a mixture); Phthalic acid derivatives such as dimethyl phthalate, diethyl phthalate, dibutyl phthalate, di-(2-ethylhexyl) phthalate, di-n-octyl phthalate, diisobutyl phthalate, diheptyl phthalate, diphenyl phthalate, diisodecyl phthalate, ditridecyl phthalate, diundecyl phthalate, dibenzyl phthalate, butyl benzyl phthalate, dinonyl phthalate, and dicyclohexyl phthalate; Isophthalic acid derivatives such as dimethyl isophthalate, di-(2-ethylhexyl) isophthalate, and diisooctyl isophthalate; Tetrahydrophthalic acid derivatives such as di-(2-ethylhexyl)tetrahydrophthalate, di-n-octyltetrahydrophthalate, and diisodecyltetrahydrophthalate; Adipic acid derivatives such as di-n-butyl adipate, di-(2-ethylhexyl) adipate, diisodecyl adipate, diisononyl adipate; Azelaic acid derivatives such as di-(2-ethylhexyl) azelate, diisooctyl azelate, di-n-hexyl azelate; Sebacic acid derivatives such as di-n-butyl sebacate, di-(2-ethylhexyl) sebacate, diisodecyl sebacate, di-(2-butyloctyl) sebacate; Maleic acid derivatives such as di-n-butyl maleate, dimethyl maleate, diethyl maleate, di-(2-ethylhexyl) maleate; Fumaric acid derivatives such as di-n-butyl fumarate, di-(2-ethylhexyl) fumarate; Citric acid derivatives such as triethyl citrate, tri-n-butyl citrate, acetyl triethyl citrate, acetyl tri-(2-ethylhexyl) citrate; Itaconic acid derivatives such as monomethyl itaconate, monobutyl itaconate, dimethyl itaconate, diethyl itaconate, dibutyl itaconate, and di-(2-ethylhexyl) itaconate; Oleic acid derivatives such as butyl oleate, glyceryl monooleate, and diethylene glycol monooleate; Ricinoleic acid derivatives such as methyl acetylricinoleate, butyl acetylricinoleate, glyceryl monoricinoleate, diethylene glycol monoricinoleate; Stearic acid derivatives such as n-butyl stearate and diethylene glycol distearate (but excluding 12-hydroxystearic acid and its esters); Other fatty acid derivatives such as diethylene glycol monolaurate, diethylene glycol dipelargonate, and pentaerythritol fatty acid esters; Phosphoric acid derivatives such as triethyl phosphate, tributyl phosphate, tri-(2-ethylhexyl) phosphate, tributoxyethyl phosphate, triphenyl phosphate, cresyl diphenyl phosphate, tricresyl phosphate, trixylenyl phosphate, tris(chloroethyl) phosphate; Glycol derivatives such as diethylene glycol dibenzoate, dipropylene glycol dibenzoate, triethylene glycol dibenzoate, triethylene glycol di-(2-ethylbutyrate), triethylene glycol di-(2-ethylhexoate), dibutylmethylene bisthioglycolate; Glycerin derivatives such as glycerol monoacetate, glycerol triacetate, and glycerol tributyrate; Epoxy derivatives such as epoxy diisodecyl hexahydrophthalate, epoxy triglyceride, epoxidized octyl oleate, epoxidized decyl oleate; Polyester plasticizers such as adipic acid polyesters, sebacic acid polyesters, and phthalic acid polyesters; etc.

[0066] Examples of the so-called secondary plasticizers include chlorinated paraffin, fatty acid esters of glycols such as triethylene glycol dicaprylate, butyl epoxy stearate, phenyl oleate, and methyl dihydroabietic acid.

[0067] These plasticizers may be used alone or in combination of two or more of them, such as a primary plasticizer and a secondary plasticizer. When a secondary plasticizer is used, it is preferable to use a primary plasticizer in an amount equal to or greater than the mass of the secondary plasticizer.

[0068] Among the above-mentioned plasticizers, from the viewpoint of improving the moldability of the vinyl chloride resin composition, it is preferable to use trimellitic acid esters and / or pyromellitic acid esters, it is more preferable to use trimellitic acid esters, it is even more preferable to use linear trimellitic acid esters, and it is even more preferable to use linear trimellitic acid esters having two or more alkyl groups with different carbon numbers in the molecule. The number of carbon atoms of the alkyl group is preferably 8 to 10, and it is more preferable that the alkyl group is an n-octyl group or an n-decyl group. It is also preferable to further use epoxidized soybean oil together with the above trimellitic acid esters.

[0069] -SP value- The SP value of the plasticizer used in the polyvinyl chloride resin composition is 7 (cal / cm 3 ) 1 / 2 It is preferable that the calorie content is 8 (cal / cm 3 ) 1 / 2 More preferably, it is 12 (cal / cm 3 ) 1 / 2 It is preferable that the calorie content is 10 (cal / cm 3 ) 1 / 2 It is more preferable that the SP value is not more than 1. When the SP value of the plasticizer used in the vinyl chloride resin is within the above-mentioned range, migration of the plasticizer from the vinyl chloride resin molded sheet can be more effectively suppressed.

[0070] [Additives] The vinyl chloride resin composition may further contain various additives in addition to the above-mentioned components. The additives are not particularly limited, and include lubricants such as silicone oil, stabilizers such as perchloric acid-treated hydrotalcite, zeolite, β-diketone, and fatty acid metal salts, release agents, dusting agents other than the above-mentioned vinyl chloride resin fine particles, and other additives.

[0071] -Silicone oil- Examples of silicone oils that may be contained in the vinyl chloride resin composition include ether-modified silicone oils, fatty acid amide-modified silicone oils, and unmodified silicone oils.

[0072] Here, the content of silicone oil is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, more preferably 0.15 parts by mass or more, more preferably 1.5 parts by mass or less, more preferably 1.0 parts by mass or less, more preferably 0.5 parts by mass or less, and even more preferably 0.4 parts by mass or less, relative to 100 parts by mass of the vinyl chloride resin.If the content of silicone oil is above the lower limit, the stickiness of the surface of the vinyl chloride resin molded sheet can be sufficiently reduced to improve the surface slipperiness.In addition, if the content of silicone oil is below the upper limit, for example, even when the vinyl chloride resin molded sheet is continuously molded, the surface of the mold or the like can be prevented from being contaminated due to an excessive amount of silicone oil.

[0073] -Perchloric acid treated hydrotalcite- The perchloric acid-treated hydrotalcite that may be contained in the vinyl chloride resin composition is prepared by, for example, adding the hydrotalcite to a dilute aqueous solution of perchloric acid, stirring, and then filtering, dehydrating, or drying as necessary to remove the carbonate anions (CO 2- ) to convert at least a portion of the - ) (2 moles of perchlorate anion are substituted for 1 mole of carbonate anion), it is possible to easily produce perchloric acid-introduced hydrotalcite. The molar ratio of the hydrotalcite to the perchloric acid can be set arbitrarily, but generally, it is preferable to use 0.1 moles or more and 2 moles or less of perchloric acid per mole of hydrotalcite.

[0074] Here, the substitution rate of carbonate anions to perchlorate anions in untreated (unsubstituted with no perchlorate anion introduced) hydrotalcite is preferably 50 mol% or more, more preferably 70 mol% or more, and even more preferably 85 mol% or more. In addition, the substitution rate of carbonate anions to perchlorate anions in untreated (unsubstituted with no perchlorate anion introduced) hydrotalcite is preferably 95 mol% or less. When the substitution rate of carbonate anions to perchlorate anions in untreated (unsubstituted with no perchlorate anion introduced) hydrotalcite is within the above range, a vinyl chloride resin molded sheet can be more easily produced.

[0075] Hydrotalcite has the general formula: [Mg 1-x Al x (OH)2] x+ [(CO3) x / 2 mH2O] x- A nonstoichiometric compound represented by the formula: 1-x Al x (OH)2] x+ and the negatively charged intermediate layer [(CO3) x / 2 mH2O] x- It is an inorganic substance having a layered crystal structure consisting of Mg6Al2(OH). In the above general formula, x is a number greater than 0 and less than or equal to 0.33. Natural hydrotalcite is Mg6Al2(OH) 16 CO3·4H2O. Synthetic hydrotalcites include Mg 4.5 Al2(OH) 13 CO3·3.5H2O is commercially available. A method for synthesizing synthetic hydrotalcite is described, for example, in JP-A-61-174270.

[0076] Here, the content of the perchloric acid-treated hydrotalcite is not particularly limited, and is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and preferably 7 parts by mass or less, and more preferably 6 parts by mass or less, relative to 100 parts by mass of the vinyl chloride resin. If the content of the perchloric acid-treated hydrotalcite is within the above range, the vinyl chloride resin molded sheet obtained by molding the vinyl chloride resin composition can better maintain tensile elongation at low temperatures.

[0077] -Zeolite- The vinyl chloride resin composition may contain zeolite as a stabilizer. Zeolite is represented by the general formula: M x / n ·[(AlO2) x (SiO2) y ]·zH2O (where M is a metal ion of valence n, x+y is the number of tetrahedra per monolayer, and z is the number of moles of water). The types of M in the formula include monovalent or divalent metals such as Na, Li, Ca, Mg, and Zn, and mixtures of these.

[0078] Here, the content of zeolite is not particularly limited, but is preferably 0.1 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the vinyl chloride resin.

[0079] -β-diketone- The β-diketone is used to more effectively suppress the variation in the initial color tone of the vinyl chloride resin molded sheet obtained by molding the vinyl chloride resin composition. Specific examples of the β-diketone include dibenzoylmethane, stearoylbenzoylmethane, palmitoylbenzoylmethane, etc. These β-diketones may be used alone or in combination of two or more.

[0080] The content of the β-diketone is not particularly limited, but is preferably 0.01 parts by mass or more and 5 parts by mass or less relative to 100 parts by mass of the vinyl chloride resin.

[0081] -Fatty acid metal salts- The fatty acid metal salt that the vinyl chloride resin composition may contain is not particularly limited and may be any fatty acid metal salt. Among them, monovalent fatty acid metal salts are preferred, monovalent fatty acid metal salts having 12 to 24 carbon atoms are more preferred, and monovalent fatty acid metal salts having 15 to 21 carbon atoms are even more preferred. Specific examples of fatty acid metal salts include lithium stearate, magnesium stearate, aluminum stearate, calcium stearate, strontium stearate, barium stearate, zinc stearate, calcium laurate, barium laurate, zinc laurate, barium 2-ethylhexanoate, zinc 2-ethylhexanoate, barium ricinoleate, and zinc ricinoleate. As the metal constituting the fatty acid metal salt, metals capable of generating polyvalent cations are preferred, metals capable of generating divalent cations are more preferred, metals capable of generating divalent cations in the third to sixth periods of the periodic table are even more preferred, and metals capable of generating divalent cations in the fourth period of the periodic table are particularly preferred. The most preferred fatty acid metal salt is zinc stearate.

[0082] Here, the content of the fatty acid metal salt is not particularly limited, and is preferably 0.01 parts by mass or more, more preferably 0.03 parts by mass or more, and preferably 5 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less, relative to 100 parts by mass of the vinyl chloride resin. If the content of the fatty acid metal salt is within the above range, the color difference value of the vinyl chloride resin molded sheet obtained by molding the vinyl chloride resin composition can be reduced.

[0083] -Release agent- The release agent is not particularly limited, and examples thereof include 12-hydroxystearic acid-based lubricants such as 12-hydroxystearic acid, 12-hydroxystearic acid esters, and 12-hydroxystearic acid oligomers. The content of the release agent is not particularly limited, and can be 0.01 parts by mass or more and 5 parts by mass or less with respect to 100 parts by mass of the vinyl chloride resin.

[0084] -Other dusting agents- Other dusting agents that may be contained in the vinyl chloride resin composition other than the vinyl chloride resin fine particles include inorganic fine particles such as calcium carbonate, talc, and aluminum oxide; and organic fine particles such as polyacrylonitrile resin fine particles, poly(meth)acrylate resin fine particles, polystyrene resin fine particles, polyethylene resin fine particles, polypropylene resin fine particles, polyester resin fine particles, and polyamide resin fine particles. Among these, inorganic fine particles having an average particle size of 10 nm or more and 100 nm or less are preferred.

[0085] The content of the other dusting agent is not particularly limited, and is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, based on 100 parts by mass of the vinyl chloride resin. The other dusting agents may be used alone or in combination of two or more kinds, or may be used in combination with the above-mentioned vinyl chloride resin fine particles.

[0086] -Other additives- Other additives that may be contained in the vinyl chloride resin composition are not particularly limited, and examples thereof include colorants (pigments), impact resistance modifiers, perchlorate compounds other than perchlorate-treated hydrotalcite (sodium perchlorate, potassium perchlorate, etc.), epoxidized vegetable oil-based heat stabilizers such as epoxidized soybean oil and epoxidized linseed oil; antioxidants, mildew inhibitors, flame retardants, antistatic agents, fillers, light stabilizers, and foaming agents.

[0087] Specific examples of the colorant (pigment) are quinacridone pigments, perylene pigments, polyazo condensation pigments, isoindolinone pigments, copper phthalocyanine pigments, titanium white, and carbon black. One or more pigments are used. Quinacridone pigments are produced by treating p-phenylenedianthranilic acids with concentrated sulfuric acid, and exhibit a yellowish red to reddish purple hue. Specific examples of quinacridone pigments include quinacridone red, quinacridone magenta, and quinacridone violet. Perylene pigments are obtained by the condensation reaction of perylene-3,4,9,10-tetracarboxylic anhydride with aromatic primary amines, and exhibit hues ranging from red to reddish purple to brown. Specific examples of perylene pigments include perylene red, perylene orange, perylene maroon, perylene vermilion, and perylene bordeaux. Polyazo condensation pigments are obtained by condensing an azo dye in a solvent to increase the molecular weight, and exhibit yellow or red pigment hues. Specific examples of polyazo condensation pigments include polyazo red, polyazo yellow, chromophthal orange, chromophthal red, and chromophthal scarlet. Isoindolinone pigments are obtained by the condensation reaction of 4,5,6,7-tetrachloroisoindolinone with aromatic primary diamines, and exhibit a greenish yellow to red or brown hue. A specific example of an isoindolinone pigment is isoindolinone yellow. Copper phthalocyanine pigments are pigments in which copper is coordinated with phthalocyanines, and they exhibit hues ranging from yellowish green to vivid blue. Specific examples of copper phthalocyanine pigments are phthalocyanine green and phthalocyanine blue. Titanium white is a white pigment made of titanium dioxide, has great hiding power, and is available in anatase and rutile types. Carbon black is a black pigment whose main component is carbon and which also contains oxygen, hydrogen, and nitrogen. Specific examples of carbon black include thermal black, acetylene black, channel black, furnace black, lamp black, and bone black.

[0088] Specific examples of impact modifiers include acrylonitrile-butadiene-styrene copolymers, methyl methacrylate-butadiene-styrene copolymers, chlorinated polyethylene, ethylene-vinyl acetate copolymers, and chlorosulfonated polyethylene. In the vinyl chloride resin composition, one or more impact modifiers can be used. The impact modifier is dispersed in the vinyl chloride resin composition as a heterogeneous phase of fine elastic particles. In the vinyl chloride resin composition, the chains and polar groups graft-polymerized to the elastic particles are compatible with the vinyl chloride resin, and the impact resistance of the vinyl chloride resin molded sheet obtained by molding the vinyl chloride resin composition is improved.

[0089] Specific examples of the antioxidant include phenol-based antioxidants, sulfur-based antioxidants, and phosphorus-based antioxidants such as phosphites.

[0090] Specific examples of the antifungal agent include aliphatic ester-based antifungal agents, hydrocarbon-based antifungal agents, organic nitrogen-based antifungal agents, and organic nitrogen sulfur-based antifungal agents.

[0091] Specific examples of the flame retardant include halogen-based flame retardants; phosphorus-based flame retardants such as phosphate esters; and inorganic hydroxides such as magnesium hydroxide and aluminum hydroxide.

[0092] Specific examples of the antistatic agent include anionic antistatic agents such as fatty acid salts, higher alcohol sulfates, and sulfonates; cationic antistatic agents such as aliphatic amine salts and quaternary ammonium salts; and nonionic antistatic agents such as polyoxyethylene alkyl ethers and polyoxyethylene alkylphenol ethers.

[0093] Specific examples of fillers include silica, talc, mica, calcium carbonate, clay, and the like.

[0094] Specific examples of the light stabilizer include ultraviolet absorbers such as benzotriazole-based, benzophenone-based and nickel chelate-based light stabilizers, and hindered amine-based light stabilizers.

[0095] Specific examples of blowing agents include organic blowing agents such as azo compounds such as azodicarbonamide and azobisisobutyronitrile, nitroso compounds such as N,N'-dinitrosopentamethylenetetramine, and sulfonyl hydrazide compounds such as p-toluenesulfonyl hydrazide and p,p-oxybis(benzenesulfonyl hydrazide); gas-based blowing agents such as volatile hydrocarbon compounds such as chlorofluorocarbon gas, carbon dioxide gas, water, and pentane, and microcapsules containing these compounds; and the like.

[0096] [Method for preparing vinyl chloride resin composition] The vinyl chloride resin composition is not particularly limited and can be prepared by mixing the above-mentioned components. Here, the method of mixing the vinyl chloride resin, the plasticizer, and various additives further used as necessary is not particularly limited, and for example, the components other than the dusting agent containing the vinyl chloride resin fine particles are mixed by dry blending, and then the dusting agent is added and mixed. Here, it is preferable to use a Henschel mixer for dry blending. In addition, the temperature during dry blending is not particularly limited, and is preferably 50°C or higher, more preferably 70°C or higher, and preferably 200°C or lower.

[0097] <<Method of forming polyvinyl chloride resin sheets>> The vinyl chloride resin molded sheet is obtained by molding the vinyl chloride resin composition into a sheet. The method for molding the vinyl chloride resin composition is not particularly limited and any known molding method can be used, but it is preferable to use powder molding, and more preferable to use powder slush molding. Here, the mold temperature during powder slush molding is not particularly limited, but is preferably 200°C or higher, more preferably 220°C or higher, and is preferably 300°C or lower, and more preferably 280°C or lower.

[0098] When producing a vinyl chloride resin molded sheet, the following method can be used, without any particular limitation. That is, the vinyl chloride resin composition of the present invention is sprinkled onto a mold having a temperature in the above range, and the mold is left for 5 to 30 seconds, after which the excess vinyl chloride resin composition is shaken off, and the mold is further left for 30 seconds to 3 minutes at an arbitrary temperature. The mold is then cooled to 10°C to 60°C, and the obtained vinyl chloride resin molded sheet is demolded from the mold. The demolded vinyl chloride resin molded sheet is obtained, for example, as a sheet-shaped molded body that follows the shape of the mold. The thickness of the obtained polyvinyl chloride resin molded sheet is not particularly limited, but is preferably 0.8 mm or more, more preferably 1.0 mm or more, and is preferably 1.6 mm or less, more preferably 1.4 mm or less.

[0099] <Resin layer L> The vinyl chloride resin laminate sheet of the present invention has a predetermined resin layer L arranged on at least one side in the thickness direction of the vinyl chloride resin molded sheet described above. The predetermined resin layer L may be arranged on both sides in the thickness direction of the vinyl chloride resin molded sheet, or may be arranged on only one side in the thickness direction of the vinyl chloride resin molded sheet, but is usually arranged on only one side in the thickness direction of the vinyl chloride resin molded sheet.

[0100] Furthermore, the surface on one or both sides in the thickness direction of the vinyl chloride resin laminate sheet may be partially or entirely composed of a predetermined resin layer L.

[0101] Here, the predetermined resin layer L is usually directly bonded to the vinyl chloride resin molded sheet.

[0102] The predetermined resin layer L is formed using the above-mentioned resin layer-forming composition. Here, the organometallic compound contained in the resin layer-forming composition is consumed in the reaction that crosslinks the polymers that make up the resin A, but some of it may remain in the formed resin layer L. Resin A contained in the composition for forming a resin layer is also contained in resin layer L, but in resin layer L, at least a portion of the polymers constituting resin A are crosslinked by a structure derived from an organometallic compound. The resin layer L also contains components other than the resin A and the organometallic compound contained in the resin layer-forming composition. In addition, since the solvent contained in the composition for forming a resin layer is removed by a drying process or the like described below, the solvent is usually not contained in the resin layer L that is formed, but it is acceptable for the solvent to remain in the resin layer L within the range in which the desired effects of the present invention are obtained.

[0103] Here, it is generally believed that when a vinyl chloride resin molded sheet is placed in direct contact with other resin members such as, for example, a urethane foam molded body, the plasticizer in the vinyl chloride resin molded sheet migrates to the other resin members, reducing the amount of plasticizer in the vinyl chloride resin molded sheet, and causing deterioration of the vinyl chloride resin molded sheet. However, if the vinyl chloride resin laminated sheet of the present invention has a resin layer L containing a resin A having the above-mentioned SP value in a predetermined range, by interposing the resin layer L between the vinyl chloride resin molded sheet and other resin members, it becomes difficult for the plasticizer to pass through the resin layer L from the vinyl chloride resin molded sheet to reach other resin members, etc., and as a result, it is presumed that the migration of the plasticizer from the vinyl chloride resin molded sheet can be well suppressed. In addition, the resin A contained in the resin layer forming composition usually has low moist heat resistance, but by further including an organometallic compound in the resin layer forming composition, in the resin layer L formed, at least a portion of the polymers constituting the resin A are crosslinked by a structure derived from the organometallic compound, so that the resin layer L becomes insoluble in solvents such as water, thereby increasing the moist heat resistance of the resin layer L.

[0104] <<Thickness>> The thickness of the resin layer L is preferably 0.1 μm or more, more preferably 1 μm or more, even more preferably 5 μm or more, particularly preferably 10 μm or more, and preferably 1000 μm or less, more preferably 100 μm or less, even more preferably 50 μm or less, and particularly preferably 30 μm or less. If the thickness of the resin layer L is 0.1 μm or more, the migration of the plasticizer from the vinyl chloride resin molded sheet can be more effectively suppressed. On the other hand, if the thickness of the resin layer L is 1000 μm or less, the weight of the entire resin layer L can be reduced.

[0105] <<Method of forming resin layer L>> The resin layer L is formed on at least one side in the thickness direction of the vinyl chloride resin molded sheet. Here, examples of the method for forming the resin layer L on at least one side in the thickness direction of the vinyl chloride resin molded sheet include the following methods. 1) A method in which a resin layer-forming composition is applied to at least one side of a vinyl chloride resin molded sheet, followed by drying; 2) A method of immersing a vinyl chloride resin molded sheet in a resin layer-forming composition and then drying the same; and 3) A method in which a resin layer-forming composition is applied onto a release substrate, and dried to prepare a resin layer L, and the obtained resin layer L is transferred and laminated onto at least one side of a vinyl chloride resin molded sheet. Among these, the method 1) is particularly preferred because it is easy to control the thickness of the resin layer L. The method 1) specifically includes a step of applying a resin layer-forming composition to at least one side of a vinyl chloride resin molded sheet (application step), and a step of drying the applied resin layer-forming composition to form the resin layer L (resin layer formation step).

[0106] [Coating process] In the coating step, the method for coating the resin layer-forming composition on at least one side of the vinyl chloride resin molded sheet is not particularly limited, and examples thereof include a bar coating method, a doctor blade method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, a brush coating method, a spray coating method, etc. Among these, it is preferable to use the spray coating method, since it is easy to deal with cases where the vinyl chloride resin molded sheet has a complicated structure such as a curved shape.

[0107] [Resin layer formation process] In addition, in the resin layer forming step, examples of the method for drying the applied resin layer forming composition include drying with warm air, hot air, or low humidity air, vacuum drying, and drying by irradiation with infrared rays or electron beams. By drying the applied resin layer forming composition, a crosslinking reaction occurs between the resin A and the organometallic compound, and the polymers constituting the resin A are crosslinked with each other via the organometallic compound. This can improve the moist heat resistance of the resin layer L to be formed. The drying conditions are not particularly limited, but the drying temperature is preferably 10°C or higher, more preferably 20°C or higher, even more preferably 30°C or higher, particularly preferably 40°C or higher, and preferably 150°C or lower, more preferably 110°C or lower, and even more preferably 70°C or lower. If the drying temperature is above the lower limit, the drying efficiency is improved and the crosslinking reaction is promoted. On the other hand, if the drying temperature is below the upper limit, no pinholes are generated in the resin layer, and a uniform resin layer is formed. In addition, the drying time can be arbitrarily adjusted within a range in which the desired effect of the present invention can be obtained.

[0108] (Method of manufacturing polyvinyl chloride resin laminate sheet) The method for producing a vinyl chloride resin laminate sheet of the present invention is characterized by comprising a coating step of coating the above-mentioned resin layer-forming composition on at least one side in the thickness direction of a vinyl chloride resin molded sheet containing a vinyl chloride resin and a plasticizer, and a resin layer-forming step of drying the applied resin layer-forming composition to form a resin layer L. According to the method for producing a vinyl chloride resin laminate sheet of the present invention, it is possible to produce a vinyl chloride resin laminate sheet that can effectively suppress migration of the plasticizer from the vinyl chloride resin molded sheet and has a resin layer L with excellent wet heat resistance.

[0109] Here, as the vinyl chloride resin molded sheet used in the method for producing a vinyl chloride resin laminate sheet of the present invention, the vinyl chloride resin molded sheet described above in the section "Vinyl chloride resin laminate sheet" can be used. Also, as the resin layer forming composition used in the method for producing a vinyl chloride resin laminate sheet of the present invention, the resin layer forming composition of the present invention described above can be used. In addition, as the coating step and the resin layer forming step in the manufacturing method of the vinyl chloride resin laminate sheet of the present invention, for example, the coating step and the resin layer forming step included in the method for forming the resin layer L described above in the section "Vinyl chloride resin laminate sheet" can be carried out, respectively.

[0110] (Laminate) The laminate of the present invention has a polyurethane foam molded body and the vinyl chloride resin laminate sheet described above. The laminate of the present invention has a structure in which the above-mentioned predetermined resin layer L is interposed between the polyurethane foam molded body and the vinyl chloride resin molded sheet. Usually, the polyurethane foam molded body is backed on one side of the vinyl chloride resin laminate sheet with the resin layer L interposed therebetween, and the polyurethane foam molded body and the vinyl chloride resin laminate sheet are adjacent to each other in the lamination direction (i.e., the polyurethane foam molded body and the vinyl chloride resin molded sheet are laminated in the lamination direction via the resin layer L).

[0111] In addition, since the laminate of the present invention has the resin layer L between the urethane foam molded body and the vinyl chloride resin molded sheet, migration of the plasticizer from the vinyl chloride resin molded sheet can be effectively suppressed and the laminate of the present invention has excellent moist heat resistance. Therefore, the laminate of the present invention is preferably used as an automobile interior material for automobile interior parts such as automobile instrument panels and door trims, and is particularly preferably used for automobile instrument panels.

[0112] Here, the lamination method is not particularly limited, and for example, the following method can be used: That is, isocyanates and polyols, which are raw materials for the polyurethane foam, are reacted and polymerized on the surface of the vinyl chloride resin laminate sheet on the side where the resin layer L is provided, and polyurethane is foamed by a known method, thereby directly forming a polyurethane foam on the vinyl chloride resin laminate sheet. The SP value of the polyurethane resin that constitutes the polyurethane foam is usually 8 (cal / cm 3 ) 1 / 2 More preferably, 9 (cal / cm 3) 1 / 2 More than 12 (cal / cm 3 ) 1 / 2 It is preferably 11 (cal / cm 3 ) 1 / 2 The following is the result. EXAMPLES

[0113] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following description, the units "%" and "parts" expressing amounts are by mass unless otherwise specified. The storage stability of the resin layer-forming composition, the thickness and moist heat resistance of the resin layer L, and the reduction rate of the plasticizer in the vinyl chloride resin molded sheet after heating were measured or evaluated by the following methods.

[0114] <Storage Stability of Resin Layer-Forming Composition> In each of the Examples and Comparative Examples, the resin layer forming composition was prepared and then allowed to stand for one week under the condition of 23° C. Thereafter, the resin layer forming composition was visually observed, and the storage stability was evaluated according to the following criteria. The less precipitate observed in the resin layer forming composition, the more excellent the storage stability of the resin layer forming composition. A: No precipitate was observed in the resin layer forming composition. B: A small amount of precipitate is observed in the resin layer forming composition. C: Precipitates are clearly observed in the resin layer forming composition.

[0115] <Thickness of resin layer L> The cross section of the resin layer L of the laminate obtained in each of the Examples and Comparative Examples was observed with a digital microscope ("VHX-900" manufactured by KEYENCE Corporation) to measure the thickness of the resin layer L. The cross section was observed and the thickness was measured at three points in total, one point near each of the long sides of the laminate and one point near the center of the surface of the laminate, and the smallest value was recorded as the measurement result.

[0116] <Moisture and heat resistance of resin layer L> A moist heat resistance test was conducted by leaving the vinyl chloride resin laminate sheets obtained in each Example and Comparative Example at rest for 300 hours under conditions of a temperature of 80°C and a humidity of 80% RH. Thereafter, the surface of the resin layer L side of the vinyl chloride resin laminate sheet was visually observed, and the moist heat resistance of the resin layer L was evaluated according to the following criteria. The fewer droplets observed, the more difficult it is for the resin layer L to dissolve under high humidity and high temperature conditions, indicating that it has excellent moist heat resistance. A: The resin layer L is not dissolved at all, and no droplets are observed. B: The resin layer L is slightly melted, and a few droplets are observed. C: The resin layer L is clearly melted, and many droplets are observed.

[0117] <Reduction rate of plasticizer in polyvinyl chloride resin molded sheet before and after heating> Only the vinyl chloride resin molded sheet was peeled off from the laminate obtained in each Example and Comparative Example, and 50±0.2 mg was taken from the vinyl chloride resin molded sheet and dissolved in tetrahydrofuran (THF). After the volume was increased to 50 mL with methanol, the supernatant solution was analyzed by HPLC (high performance liquid chromatography) under the following conditions to measure the content ratio A (%) of the plasticizer in the vinyl chloride resin molded sheet before heating.

[0118] High-performance liquid chromatograph: Agilent LC1260-II Column: Agilent "ZORBAX Eclipse XDB-C8" Column temperature: 40℃ Mobile phase A: Acetonitrile Mobile phase B: Ion-exchanged water Gradient conditions: 0 min (20% by volume mobile phase B), 2.5 min (0% by volume mobile phase B), 8.0 min (0% by volume mobile phase B) Flow rate: 1.0mL / min Detector: Diode array detector (DAD) Signal: 254nm Reference: 360nm Injection amount: 1μm

[0119] In addition, the laminate obtained in each of the Examples and Comparative Examples was placed in an oven and heated in an environment at a temperature of 130°C for 100 hours, and the plasticizer content B (%) in the vinyl chloride resin molded sheet after heating was measured in the same manner as described above, except that the laminate was placed in an oven and heated in an environment at a temperature of 130°C for 100 hours.

[0120] From the above, when a polyvinyl chloride resin molded sheet having a content of other components (such as polyvinyl chloride resin) other than plasticizer of W (g) is heated under the above-mentioned conditions, the content (g) and content ratio (%) of each of the plasticizer and other components in the polyvinyl chloride resin molded sheet before and after heating are shown in Table 1 using the above A, B, and W. Therefore, the reduction rate X (%) of the plasticizer was calculated by the following calculation formula (I). Note that the content W (g) of other components in the polyvinyl chloride resin molded sheet does not change before and after heating.

[0121] [Table 1]

[0122] Plasticizer reduction rate X(%) = 100 × {(plasticizer content before heating) - (plasticizer content after heating)} / (plasticizer content before heating) =100×{W×A / (100-A)-W×B / (100-B)} / [W×A / (100-A)] =100×[1-{B×(100-A)} / {A×(100-B)}]···(I)

[0123] Example 1 <Preparation of vinyl chloride resin composition> Of the ingredients shown in Table 2, the ingredients other than the plasticizer (trimellitic acid ester), the epoxidized soybean oil as a stabilizer, and the vinyl chloride resin fine particles as a dusting agent were mixed in a Henschel mixer. Then, when the temperature of the mixture rose to 80°C, all of the plasticizer and the epoxidized soybean oil as a stabilizer were added, and the temperature was further raised to dry up (referring to a state in which the plasticizer is absorbed into the vinyl chloride resin particles as the vinyl chloride resin and the mixture becomes smooth). Thereafter, when the dried-up mixture was cooled to a temperature of 100°C or less, the vinyl chloride resin fine particles as a dusting agent were added, and a vinyl chloride resin composition was prepared.

[0124] <Formation of polyvinyl chloride resin molded sheet> The vinyl chloride resin composition obtained above was sprinkled onto a textured mold heated to a temperature of 250°C, and was left to melt for an arbitrary time of about 8 to 20 seconds, after which the excess vinyl chloride resin composition was shaken off. The textured mold onto which the vinyl chloride resin composition had been sprinkled was then left to stand in an oven set at a temperature of 200°C, and after 60 seconds had elapsed since being left to stand, the textured mold was cooled with cooling water. When the mold temperature was cooled to 40°C, a vinyl chloride resin molded sheet of 200mm x 300mm x 1.2mm was removed from the mold.

[0125] <Preparation of Resin Layer-Forming Composition> Into a vessel, 230 parts of water as a solvent, 360 parts of isopropyl alcohol (Kanto Chemical Co., Ltd.), 5 parts of methyl polyglycol (number average degree of polymerization: 4) as a plasticizer for the resin layer, and 10 parts of polyoxyethylene polyoxypropylene alkyl (C12-14) ether (Kao Corporation "Emulgen LS-114") as a dispersant were added, and stirring was started at room temperature (23°C). Polyvinyl alcohol (PVA, Nippon Acetic Acid & Poval Co., Ltd. "JMR-20M") as resin A, saponification degree from polyvinyl acetate: 65%, average degree of polymerization: 400, SP value: 16.4 (cal / cm 3 ) 1 / 2) was added, and heating was started while stirring. The mixture was heated to about 45°C, and when the PVA was dissolved, heating was stopped, and the mixture was allowed to cool to about room temperature while stirring. Thereafter, 5 parts of yellowing polyester polyurethane (Dai-ichi Kogyo Seiyaku Co., Ltd.'s "Superflex (registered trademark) 740") was added as a binder while stirring, and 4.10 parts of dihydroxybis (ammonium lactate) titanium (Matsumoto Fine Chemical Co., Ltd.'s "Orgatics TC-300") was added as an organometallic compound, in terms of dry mass, and mixed to prepare a composition for forming a resin layer. The storage stability of the obtained composition for forming a resin layer was evaluated. The results are shown in Table 3.

[0126] <Preparation of polyvinyl chloride resin laminate sheet (formation of resin layer L)> The resin layer forming composition obtained by the above method was sprayed onto the surface opposite to the textured surface of the obtained vinyl chloride resin molded sheet. Thereafter, the vinyl chloride resin molded sheet was dried for one day with hot air at 40°C to produce a vinyl chloride resin laminate sheet having a resin layer L formed on one side of the vinyl chloride resin molded sheet. In addition, the obtained vinyl chloride resin laminate sheet was used to evaluate the moist heat resistance of the resin layer L. The results are shown in Table 3.

[0127] <Formation of Laminate> The polyvinyl chloride resin laminate sheet thus produced was left to stand in an oven set at a temperature of 100° C. for 2 hours, and then placed in a mold measuring 200 mm×300 mm×10 mm with the textured surface facing down. Separately, 50 parts of propylene glycol PO (propylene oxide)·EO (ethylene oxide) block adduct (hydroxyl value 28, terminal EO unit content = 10%, internal EO unit content 4%), 50 parts of glycerin PO·EO block adduct (hydroxyl value 21, terminal EO unit content = 14%), 2.5 parts of water, 0.2 parts of ethylene glycol solution of triethylenediamine (manufactured by Tosoh Corporation, product name "TEDA-L33"), 1.2 parts of triethanolamine, 0.5 parts of triethylamine, and 0.5 parts of foam stabilizer (manufactured by Shin-Etsu Chemical Co., Ltd., product name "F-122") were mixed to obtain a polyol mixture. In addition, the obtained polyol mixture was mixed with polymethylene polyphenylene polyisocyanate (Polymeric MDI) in a ratio such that the isocyanate index was 98 to prepare a mixed liquid. The prepared mixture was then poured onto the vinyl chloride resin laminate sheet placed in the mold as described above. Thereafter, the mold was covered with an aluminum plate measuring 348 mm × 255 mm × 10 mm to seal the mold. The mold was left for 5 minutes after sealing, and a polyurethane foam molded body (thickness: 8.78 mm, density: 0.18 g / cm) was formed adjacent to the vinyl chloride resin laminate sheet (thickness: 1.22 mm) as a skin. 3 , SP value: 10.0 (cal / cm 3 ) 1 / 2 ) backed (laminated) laminate was formed in a mold. The formed laminate was then removed from the mold, and the reduction rate of the plasticizer in the vinyl chloride resin molded sheet before and after heating was measured according to the method described above. The results are shown in Table 3. The thickness of the resin layer L was measured using the laminate, and was found to be 30 μm.

[0128] Example 2 In the preparation of the resin layer forming composition of Example 1, except that the amount of dihydroxybis(ammonium lactate)titanium used as the organometallic compound was changed from 4.10 parts to 6.15 parts, a vinyl chloride resin composition, a vinyl chloride resin molded sheet, a resin layer forming composition, a vinyl chloride resin laminated sheet, and a laminate were produced in the same manner as in Example 1, and various measurements or evaluations were performed. The results are shown in Table 3. The thickness of the resin layer L was measured and found to be 30 μm.

[0129] Example 3 In the preparation of the resin layer forming composition of Example 1, except that the amount of dihydroxybis(ammonium lactate)titanium used as the organometallic compound was changed from 4.10 parts to 12.30 parts, a vinyl chloride resin composition, a vinyl chloride resin molded sheet, a resin layer forming composition, a vinyl chloride resin laminated sheet, and a laminate were produced in the same manner as in Example 1, and various measurements or evaluations were performed. The results are shown in Table 3. The thickness of the resin layer L was measured and found to be 30 μm.

[0130] Comparative Example 1 The vinyl chloride resin composition, the vinyl chloride resin molded sheet, and the laminate were produced in the same manner as in Example 1, except that in producing the vinyl chloride resin laminate sheet in Example 1, a resin layer L was not formed on the side opposite the embossed side of the vinyl chloride resin molded sheet (i.e., a vinyl chloride resin laminate sheet was not produced), and in forming the laminate in Example 1, a vinyl chloride resin molded sheet not having a resin layer L was used as is instead of the vinyl chloride resin laminate sheet to produce the laminate. The reduction rate of the plasticizer in the vinyl chloride resin molded sheet before and after heating of the obtained laminate was measured. The results are shown in Table 3.

[0131] Comparative Example 2 In the preparation of the resin layer-forming composition of Example 1, a resin A having an average degree of polymerization of 400 and an SP value of 16.4 (cal / cm 3 ) 1 / 2Instead of 100 parts of PVA (Japan Vinyl Acetate & Poval Co., Ltd.'s "JMR-20M"), which has an average degree of polymerization of 250 and an SP value of 16.4 (cal / cm 3 ) 1 / 2 A vinyl chloride resin composition, a vinyl chloride resin molded sheet, a composition for forming a resin layer, a vinyl chloride resin laminated sheet, and a laminate were produced in the same manner as in Example 1, except that 100 parts of PVA ("JMR-10M" manufactured by Japan Vinyl Acetate & Poval Co., Ltd.) was used as the organic metal compound, dihydroxybis(ammonium lactate)titanium was not used as the organic metal compound, the amount of water used as the solvent was changed from 230 parts to 160 parts, and the amount of isopropyl alcohol used as the solvent was changed from 360 parts to 240 parts. Various measurements or evaluations were performed. The results are shown in Table 3. The thickness of the resin layer L was measured and found to be 30 μm.

[0132] Comparative Example 3 In the preparation of the resin layer forming composition of Example 1, except that dihydroxybis(ammonium lactate)titanium was not used as the organometallic compound, a vinyl chloride resin composition, a vinyl chloride resin molded sheet, a resin layer forming composition, a vinyl chloride resin laminated sheet, and a laminate were produced in the same manner as in Example 1, and various measurements or evaluations were performed. The results are shown in Table 3. The thickness of the resin layer L was measured and found to be 30 μm.

[0133] Comparative Example 4 In the preparation of the resin layer forming composition of Comparative Example 2, except that the amount of dihydroxybis(ammonium lactate)titanium used as the organometallic compound was changed from 0 parts to 6.15 parts, a vinyl chloride resin composition, a vinyl chloride resin molded sheet, a resin layer forming composition, a vinyl chloride resin laminated sheet, and a laminate were produced in the same manner as in Comparative Example 2, and various measurements or evaluations were performed. The results are shown in Table 3. The thickness of the resin layer L was measured and found to be 30 μm.

[0134] [Table 2]

[0135] 1) Product name "ZEST (registered trademark) 1700ZI" (Suspension polymerization method, SP value: 9.6 (cal / cm) manufactured by Shin-Daiichi Vinyl Corporation 3 ) 1 / 2 ) 2) Shin-Daiichi Vinyl Corporation, product name "ZEST PQLTX" (emulsion polymerization method, SP value: 9.6 (cal / cm 3 ) 1 / 2 ) 3) Tosoh Corporation, product name "Ryuron Paste (registered trademark) 860" (emulsion polymerization method, SP value: 9.6 (cal / cm 3 ) 1 / 2 ) 4) Kao Corporation, product name "Trimex N-08" (SP value: 9.0 (cal / cm 3 ) 1 / 2 ) 5) Shin-Etsu Chemical Co., Ltd., product name "X-50-1039A" 6) ADEKA, product name "ADEKA Cizer O-130S" 7) Kyowa Chemical Industry Co., Ltd., product name "Alcamizer (registered trademark) 5" 8) Mizusawa Chemical Industry Co., Ltd., product name "MIZUKALIZER DS" 9) Showa Denko Co., Ltd., product name "Karens DK-1" 10) Sakai Chemical Industry Co., Ltd., product name "SAKAI SZ2000" 11) ADEKA, product name "ADEKA STAB LS-12" 12) Dainichi Seika Chemicals Co., Ltd., product name "DA PX 1720(A) Black"

[0136] [Table 3]

[0137] From Table 3, it can be seen that by using the resin layer forming compositions of Examples 1 to 3, which contain a resin whose SP value and degree of polymerization are each equal to or greater than a specified value, and an organometallic compound, it is possible to effectively suppress the migration of plasticizer from the polyvinyl chloride resin molded sheet and to form a resin layer that has excellent moist heat resistance. On the other hand, Comparative Example 1 shows that a vinyl chloride resin molded sheet alone that does not have a resin layer L formed using the above-mentioned specified resin layer forming composition is unable to effectively suppress the migration of plasticizer from the vinyl chloride resin molded sheet. Furthermore, it can be seen that the resin layers of Comparative Examples 2 to 4, which were formed using compositions other than the above-mentioned specified resin layer-forming compositions, were able to effectively suppress the migration of plasticizer from the vinyl chloride resin molded sheet, but had poor moist heat resistance. [Industrial Applicability]

[0138] According to the present invention, it is possible to provide a resin layer-forming composition that can effectively suppress migration of a plasticizer from a vinyl chloride resin molded sheet and can form a resin layer that has excellent moist heat resistance. Furthermore, according to the present invention, it is possible to provide a polyvinyl chloride resin laminate sheet which can effectively suppress migration of a plasticizer from a polyvinyl chloride resin molded sheet and has a resin layer with excellent moist heat resistance, and a method for producing the same. Furthermore, according to the present invention, it is possible to provide a laminate which can effectively inhibit migration of plasticizer from a polyvinyl chloride resin molded sheet and has excellent resistance to moist heat.

Claims

1. A resin layer-forming composition comprising a resin A and an organometallic compound, The SP value of the resin A is 14 (cal / cm 3 ) 1 / 2 That's all. The polymerization degree of the resin A is 300 or more, The content of the organometallic compound is 4.00 parts by mass or more and 6.00 parts by mass or less relative to 100 parts by mass of the resin A, the resin A is polyvinyl alcohol, an ethylene-vinyl alcohol copolymer, polyacrylamide, polymethacrylamide, poly-N-vinylformamide, water-soluble starch, hydroxyethyl cellulose, hydroxypropyl cellulose, methyl cellulose, ethyl cellulose, or chitosan; The resin layer-forming composition, wherein the organometallic compound is a titanium chelate compound containing a hydroxycarboxylic acid and / or a salt thereof.

2. A polyvinyl chloride resin molded sheet containing a polyvinyl chloride resin and a plasticizer; A vinyl chloride resin laminate sheet having a resin layer L arranged on at least one side in a thickness direction of the vinyl chloride resin molded sheet, A vinyl chloride resin laminate sheet, wherein the resin layer L is formed using the composition for forming a resin layer according to claim 1 .

3. 3. The polyvinyl chloride resin laminate sheet according to claim 2, which is used for an automobile instrument panel skin.

4. A coating step of coating the resin layer forming composition according to claim 1 on at least one side in a thickness direction of a vinyl chloride resin molded sheet containing a vinyl chloride resin and a plasticizer; a resin layer forming step of drying the applied resin layer forming composition to form a resin layer L; A method for producing a polyvinyl chloride resin laminate sheet comprising the steps of:

5. A polyurethane foam molding; The vinyl chloride resin laminate sheet according to claim 2 or 3, A laminate having A laminate, wherein the resin layer L is disposed between the polyurethane foam molded body and the vinyl chloride resin molded sheet.

Citation Information

Patent Citations

  • JP1974094768A

  • Polyvinyl chloride group laminate

    JP1987053831A

  • Pressure-sensitive adhesive for flexible vinyl chloride resin

    JP1990091178A

  • Laminated body

    JP1993096671A

  • Tape for protecting surface of colored rubber of tire

    JP1996104852A