Polypropylene heat shrinkable film
A polypropylene heat-shrinkable film with controlled composition and processing achieves efficient separation and recycling by ensuring low natural shrinkage and specific gravity, addressing the separation challenges of existing films.
Patent Information
- Application Number
- JP2022093731
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-06-09
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2042-03-28
AI Technical Summary
Existing heat-shrinkable films for PET bottles, made from materials like polystyrene, polyester, and polyvinyl chloride, are difficult to separate from PET due to differences in specific gravity, leading to reduced recycling efficiency and quality when mixed with PET bottles.
A polypropylene heat-shrinkable film with specific gravity of 0.95 or less, exhibiting excellent low-temperature shrinkability and low natural shrinkage, achieved through controlled molecular weight distribution and composition, including ethylene or 1-butene as copolymerization components, and optimized stretching and relaxation processes.
The film provides high shrinkage rates at 90°C without wrinkles, maintains dimensional stability over time, and can be efficiently separated from PET bottles by floating, enhancing recycling efficiency and quality.
Smart Images

Figure 0007567863000005 
Figure 0007567863000006 
Figure 0007567863000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polypropylene-based heat-shrinkable film suitable for heat-shrinkable labels, a label using said film, and a package using the label. [Background technology]
[0002] Heat-shrinkable films are widely used as labels for glass and plastic bottles to prevent damage to the contents, prevent tampering, and protect the packaging and products. One application in which they are used in large quantities is as labels for PET beverage bottles. In general, when attaching heat-shrinkable films to PET bottles as labels, the PET bottles covered with the labels are transported on a conveyer line to a steam-filled tunnel, where the steam is sprayed onto the film to heat it to about 70℃ to 100℃, causing it to shrink and then be attached to the bottle. For this reason, films made of stretched polyester, polystyrene, and polyvinyl chloride, which have excellent heat-shrinkability at low temperatures, are widely used.
[0003] On the other hand, PET beverage bottles are attracting attention as a renewable resource. PET bottles are collected after use and recycled into molding resin, but since labels are made of a different plastic material than PET bottles and are printed, they must be separated from the bottles.
[0004] In other words, since the inclusion of labels in PET bottles leads to a decrease in quality when they are recycled, it is necessary to remove the labels from the bottles before recycling, but in reality, there are many cases where the labels are collected without being removed. Currently, these labels must be removed by the collector, which increases the burden on recycling. This is because polystyrene, polyester, and polyvinyl chloride have a small difference in specific gravity from PET bottles, making them difficult to separate by floating or sinking in water. Separation by floating or sinking due to the difference in specific gravity is extremely easy industrially, and in particular, PET bottles have a specific gravity of about 1.3 or more, while labels have a specific gravity of 1.0 or less, so gravity separation in water is possible. If such labels are used, even if labels are mixed in during PET bottle collection, they can be separated extremely efficiently, which not only significantly reduces the burden on collection, but also makes it possible to improve the quality of the recycled resin obtained from collected PET bottles.
[0005] In this situation, polypropylene is expected to be used because it is light, with a specific gravity of about 0.9, and can be floated and separated in water unlike PET. However, it has a problem in that it does not have sufficient shrinkability at 90°C, which is necessary to shrink it with steam.
[0006] Various proposals have been made to improve the low-temperature shrinkability. For example, in Patent Document 1, the addition of petroleum resin or polyethylene enables stretching at low temperatures and improves low-temperature shrinkage. However, the addition of petroleum resin not only increases the specific gravity and reduces the efficiency of float-sink separation, but also causes the film obtained by stretching at low temperatures to have large post-shrinkage (natural shrinkage) at room temperature, which changes the dimensions of the film, and in the case of a rolled film, deformation can easily cause problems such as printing misalignment and wrinkles during secondary processing.
[0007] In order to reduce the natural shrinkage rate, Patent Document 2 proposes a film in which the molecular weight distribution of polypropylene is controlled to be small, or the film is laminated with an amorphous resin having a high glass transition temperature, such as a cyclic olefin resin. However, these films have insufficient low-temperature shrinkability for the shrinkage rate required for beverage labels. In addition, the cyclic olefin resin has a problem of being large in specific gravity. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Patent No. 5690103 [Patent Document 2] Patent No. 4574462 [Non-patent literature]
[0009] [Non-Patent Document 1] In-situ investigation on the structural evolution of mesomorphic isotactic polypropylene in a continuous heating process: Polymer 105 (2016) 133-143 Summary of the Invention [Problem to be solved by the invention]
[0010] In order to overcome the above problems, an object of the present invention is to provide a heat-shrinkable polypropylene film having a specific gravity of 0.95 or less, excellent low-temperature shrinkability, and small natural shrinkage. [Means for solving the problem]
[0011] As a result of extensive investigations, the present inventors have found that the above problems can be solved by the means described below, and have arrived at the present invention. That is, the present invention comprises the following configuration. 1. A polypropylene-based heat-shrinkable film which is a stretched film made of a polypropylene-based resin composition and which satisfies the following (1) to (6): (1) When the film is immersed in 90° C. hot water for 10 seconds, the hot water heat shrinkage is 40% or more and 80% or less in the width direction of the film. (2) When the film is immersed in 90°C hot water for 10 seconds, the hot water heat shrinkage rate is -5% or more and 12% or less in the longitudinal direction of the film. (3) The specific gravity of the film is 0.87 or more and 0.95 or less. (4) The melting peak temperature measured by a differential scanning calorimeter has at least one melting peak in the range of 70°C or higher and 100°C or lower, and at least one melting peak in the range of more than 100°C and 170°C or lower. (5) The difference between the refractive index in the width direction (Ny) and the refractive index in the length direction (Nx), Ny-Nx, is 0.015 or more and 0.030 or less. (6) The polypropylene-based heat-shrinkable film has a natural shrinkage rate in the width direction of 0.1% or more and 3.0% or less after aging for 672 hours under an atmosphere of 40°C and 65% RH. 2. The polypropylene-based heat-shrinkable film according to 1., wherein the haze of the film is from 1% to 15%. 3. A polypropylene-based heat-shrinkable film according to 1 or 2, characterized in that the non-reverse heat flow measured by a temperature modulated scanning calorimeter has a peak in the range of 20°C or higher and 60°C or lower, and the heat absorption of the peak is 0.3 J / g or higher and 0.95 J / g or lower. 4. The polypropylene-based heat-shrinkable film according to any one of 1. to 3., wherein the refractive index Ny in the width direction is 1.490 or more and 1.530 or less. 5. The polypropylene-based heat-shrinkable film according to any one of 1. to 4., wherein the polypropylene-based heat-shrinkable film has a thickness of 12 μm or more and 100 μm or less. 6. The polypropylene-based heat-shrinkable film according to any one of 1. to 5., wherein the polypropylene-based resin composition constituting the polypropylene-based heat-shrinkable film contains ethylene or 1-butene as a copolymerization component. 7. A label using the polypropylene-based heat-shrinkable film according to any one of 1. to 6. above as a base material, and having a perforation or a pair of notches provided therein. A package comprising a ring-shaped label made of a polypropylene-based heat-shrinkable film according to any one of 1. to 6. above or a label according to 7. above, at least on a part of the outer periphery of an object to be packaged. Effect of the Invention
[0012] The polypropylene-based heat-shrinkable film of the present invention has a high shrinkage rate at 90°C, and can provide a good finish without wrinkles or insufficient shrinkage as a beverage label. In addition, since the natural shrinkage rate is small, the film has excellent practicality with little dimensional change or wrinkles even after a long time has passed since it is stored. In addition, since the specific gravity is small, it can be efficiently separated from PET bottles, and therefore has excellent recyclability. [Brief description of the drawings]
[0013] [Figure 1] 1 shows heat flow charts obtained by measuring the films of Example 1 and Comparative Example 1 with a differential scanning calorimeter, and the positions of melting peaks in the charts. [Diagram 2] 1 is a non-reverse heat flow chart obtained by measuring the films of Example 1 and Comparative Example 4 using a temperature modulated differential scanning calorimeter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The polypropylene-based heat-shrinkable film obtained by stretching the polypropylene resin composition used in the present invention must have at least one melting point (melting peak temperature) measured by a differential scanning calorimeter (DSC) in the ranges of 70°C to 100°C and more than 100°C to 170°C. Heat-shrinkable films for PET bottle labels are generally heated by steam at a temperature of 70°C to 100°C and shrink, so by having a melting point of 70°C to 100°C, the oriented crystals in the stretched film melt partially, thereby exhibiting shrinkage characteristics. On the other hand, by having a melting point of 100°C to 170°C, heat resistance can be improved and fusion and blocking during heating can be suppressed, which is preferable. In addition, it is more preferable to have a melting point in the ranges of 75°C to 97°C and 110°C to 165°C, and it is particularly preferable to have a melting point in the ranges of 80°C to 95°C and 115°C to 160°C.
[0015] As the polypropylene resin used in the present invention, not only propylene homopolymers but also copolymers of propylene and other α-olefins, polypropylenes with low stereoregularity, etc. can be suitably used. As the α-olefin copolymerization component used in the copolymer of propylene and other α-olefins, α-olefins having 2 to 8 carbon atoms, such as ethylene and 1-butene, are particularly preferred, and 1-pentene, 1-hexene, 1,4-methyl-1-pentene, etc. can also be used. In addition, the copolymer is preferably a random or block copolymer obtained by polymerizing one or more of the α-olefins exemplified above with propylene. In addition, it is desirable that the resin composition obtained by using the propylene homopolymer or propylene-α-olefin copolymer used has a specific gravity of 0.85 or more and 0.95 or less, preferably 0.86 or more and 0.93 or less, and particularly preferably 0.87 or more and 0.92 or less. Polypropylene-based resins with a specific gravity of 0.85 or less generally have very low crystallinity, so that it is difficult to obtain the required shrinkage ratio even if a stretched film is formed, which is not preferable. Furthermore, if the specific gravity is 0.95 or more, the specific gravity of the film obtained after film formation will be larger than 0.95, which is undesirable. As described above, in the present invention, it is preferable not to contain cyclic olefin resins because they increase the specific gravity and reduce the low-temperature shrinkage. Also, it is preferable not to contain petroleum resins (sometimes called hydrocarbon resins) or their hydrogenated resins because they increase the specific gravity and increase the natural shrinkage rate as described above.
[0016] The specific gravity of the polypropylene-based heat-shrinkable film obtained by stretching the unstretched sheet obtained from the polypropylene-based resin composition must be 0.87 or more and 0.95 or less. The specific gravity is more preferably 0.88 or more and 0.94 or less, and particularly preferably 0.88 or more and 0.93 or less. Using a raw material with a specific gravity of 0.87 or less is not preferable because the shrinkage rate decreases due to a decrease in crystallinity and the heat resistance decreases. In addition, if the specific gravity is more than 0.95, when the heat-shrinkable film is used as a label, the efficiency of floating and sinking separation may decrease when printing or the like is applied, which is not preferable.
[0017] The melting point of the polypropylene resin can be controlled by adjusting the type and amount of α-olefin, and in order to obtain a polypropylene resin composition having different melting point peaks in the above two temperature ranges, it is preferable to use a mixture of copolymers having different melting points in an appropriate ratio, or a block copolymer of α-olefins. The copolymerization ratio of the total α-olefins contained in the polypropylene resin composition is preferably 8 mol% or more and 24 mol% or less, and more preferably 10 mol% or more and 22 mol% or less.
[0018] The melt flow rate (MFR) of the polypropylene resin composition at 230°C is preferably in the range of 0.1 to 30 g / 10 min, more preferably in the range of 0.5 to 20 g / 10 min, and particularly preferably in the range of 1.0 to 15 g / 10 min. If the MFR is 0.1 g / min or less, the pressure during extrusion increases and streaks are likely to occur from the die, which is not preferable. If the MFR is more than 30 g / 10 min, the extrusion becomes unstable, the stress during stretching decreases, thickness unevenness increases, and the viscosity decreases, making the composition more likely to break during stretching, which is not preferable. The melt flow rate can be measured by a method conforming to JIS-K-7210.
[0019] In the present invention, various additives and fillers, such as heat stabilizers, antioxidants, light stabilizers, antistatic agents, lubricants, nucleating agents, flame retardants, pigments, dyes, calcium carbonate, barium sulfate, magnesium hydroxide, mica, talc, clay, zinc oxide, magnesium oxide, aluminum oxide, antibacterial agents, antifogging agents, additives that impart natural decomposition, etc., can be added to the resin used as necessary within a range that does not impair the characteristics. In particular, from the viewpoint of handling and the meaning of imparting slipperiness, antistatic properties, and heat blocking resistance, it is preferable to add organic lubricants such as fatty acid amides, surfactants such as fatty acid alkylamines, fatty acid alkylamine esters, and fatty acid monoglycerin esters, and antiblocking agents such as silica and PMMA. When a surfactant is added, the amount is appropriately adjusted so that the required antistatic properties are obtained with an upper limit of 20,000 ppm. When an antiblocking agent is added, the amount is adjusted to a range of 300 ppm to 10,000 ppm. If the amount of these components added exceeds the upper limit, the haze decreases and the transparency is impaired, which is not preferable. Furthermore, other thermoplastic resins, thermoplastic elastomers, rubbers, etc. may be blended within a range that does not impair the properties of the film of the present invention.
[0020] The film of the present invention may have a gas barrier resin layer such as a polypropylene resin layer of the same kind or another resin layer, for example, a layer of polyethylene, a saponified ethylene-vinyl acetate copolymer, or polyvinyl alcohol laminated on the surface thereof, so long as the properties of the film are not impaired.
[0021] The film of the present invention may be surface-treated as necessary to the extent that the characteristics of the present invention are not impaired. Examples of the surface treatment method include corona discharge treatment, plasma treatment, flame treatment, acid treatment, etc., and there is no particular limitation. It is preferable to perform corona discharge treatment, plasma treatment, or flame treatment, which can be performed continuously and can be easily performed before the winding step in the production process of this film, and corona discharge treatment is particularly preferable as a means for improving the wetting tension of the surface.
[0022] The polypropylene-based heat-shrinkable film of the present invention can be formed as a single layer, but may also have a laminated structure consisting of a skin layer and a core layer, or multiple layers greater than or equal to 10 ...
[0023] Furthermore, the thickness of the polypropylene-based heat-shrinkable film of the present invention is preferably in the range of 12 μm to 100 μm. Furthermore, the thickness of the film is more preferably in the range of 15 μm to 80 μm. If the thickness of the film is 12 μm or less, the stiffness is reduced, so that the film is likely to wrinkle when attached as a label, which is not preferable. Furthermore, if the thickness is 100 μm or more, the raw material cost of the film becomes high, which is not preferable.
[0024] The packaging body of the present invention is formed by covering at least a part of the outer periphery of the packaging object with a label obtained from the heat-shrinkable polyester film of the present invention, preferably having a perforation or a notch, and then heat-shrinking the label. Examples of the packaging object include PET bottles for beverages, various bottles, cans, plastic containers for sweets and lunch boxes, and paper boxes. In addition, when a label obtained from a heat-shrinkable polypropylene film is heat-shrunk to cover the packaging object, the label is usually heat-shrunk by about 5 to 40% to be attached to the packaging body. In addition, the label to be covered on the packaging object may or may not be printed.
[0025] As a method for producing a label, when a rectangular film is rolled up and the ends are overlapped, an organic solvent is applied slightly inward from the end of one side and bonded, or the ends are overlapped and heat-sealed using a heat seal such as a heat seal or a melt-cut seal, or heat-sealed using an ultrasonic seal, etc. may be used. In addition, various adhesives such as hot melt adhesives, ultraviolet curing adhesives, solvent-based adhesives using chloroprene, acid-modified polyolefin, chlorinated polyolefin, etc., water-based adhesives using phenolic resin, polyvinyl acetate, etc., chemical reaction type adhesives using epoxy resin, urethane resin, silicone resin, etc. may be applied to the ends of the film and bonded, and these various methods may be used depending on the processing method of the film. When bonding the ends together using an organic solvent or a liquid adhesive that can be applied to various films, a method may be used in which a solvent or adhesive is applied slightly inward from the end of one side of a rolled up film, the film is immediately rolled up, the ends are overlapped and bonded, and the tube-shaped body is cut into a label-shaped body.
[0026] As the organic solvent for adhering the polypropylene-based film of the present invention when it is made into a label, aliphatic hydrocarbons such as normal hexane, normal heptane, cyclohexane, methylcyclohexane, etc., aromatic hydrocarbons such as toluene, xylene, trimethylbenzene, etc., halogenated hydrocarbons such as methylene chloride, chloroform, etc., phenols such as phenol, furans such as tetrahydrofuran, etc., or mixtures of these solvents can be used. When cyclohexane is used as the adhesive solvent, it is preferable because it can develop higher solvent adhesion strength.
[0027] The polypropylene-based heat-shrinkable film of the present invention, when treated in 90°C hot water for 10 seconds under no load, must have a heat shrinkage rate in the width direction of the film (i.e., hot water heat shrinkage rate at 90°C) calculated from the lengths before and after shrinkage according to the following formula 1 of 40% or more and 80% or less. Heat shrinkage rate = {(length before shrinkage - length after shrinkage) / length before shrinkage} × 100 (%) Formula 1
[0028] If the hot water heat shrinkage rate in the width direction at 90°C is less than 40%, the shrinkage amount is so small that wrinkles and sagging occur in the label after heat shrinkage, which is undesirable. There is no particular limit to the upper limit of the hot water heat shrinkage rate, but the upper limit that can be achieved by the technology of the present invention is 80%. The lower limit of the hot water heat shrinkage rate in the width direction at 90°C is preferably 42% or more, more preferably 45% or more, and particularly preferably 50% or more.
[0029] In addition, the polypropylene-based heat-shrinkable film of the present invention must have a hot water heat shrinkage rate in the longitudinal direction when treated in hot water at 90°C for 10 seconds under no load, which is -5% or more and 12% or less. If the hot water heat shrinkage rate in the longitudinal direction is less than -5%, the film will expand and become distorted when used as a label, which is not preferable. If the hot water heat shrinkage rate in the longitudinal direction at 90°C exceeds 12%, the film will have large vertical shrinkage and become distorted when used as a label, which is not preferable. The more preferable range of the shrinkage rate in the longitudinal direction is -3% or more and 11% or less, and particularly preferably -1% or more and 10% or less.
[0030] The haze of the polypropylene-based heat-shrinkable film of the present invention is preferably 1% or more and 15% or less. If the haze is 15% or more, the transparency is low and the appearance is unsuitable, which is not preferable. The lower limit of the haze in the present invention is 1%, and a lower limit of 2% is sufficient for practical use. The upper limit of the haze is more preferably 12% or less, and particularly preferably 10% or less. The haze varies depending on the amount of additives such as lubricants, and the occurrence of spherulites can be suppressed and reduced by using polypropylene in which an α-olefin is copolymerized with the above-mentioned polypropylene resin composition. The haze is measured by a method conforming to JIS K 7105.
[0031] The polypropylene-based heat-shrinkable film of the present invention is required to have a natural shrinkage rate (dimensional change rate) in the width direction of 3.0% or less after aging for 672 hours under an atmosphere of 40°C and 65% RH. It is preferably 2.5% or less, more preferably 2.0% or less. By making the natural shrinkage rate at 40°C and 65% RH 3.0% or less, it is possible to reduce problems during secondary processing such as dimensional changes of the film over time when stored at room temperature or in a warehouse in summer, and wrinkles caused by shrinkage over time when stored in a rolled state and print misalignment. In particular, in the present invention, the natural shrinkage rate in the width direction, where the stretching ratio is large, tends to increase, so it is necessary to reduce it. If the natural shrinkage rate in the width direction is large. In addition to reducing the width of the film that can be used during storage, which deteriorates the yield during processing, in the rolled state, both ends of the film are not held in the width direction, so the film buckles and deforms in the roll due to natural shrinkage during storage, which is not preferable. In addition, the lower limit of the natural shrinkage rate is preferably as close to 0%, but in the case of the present invention, 0.1% is the technical lower limit.
[0032] The polypropylene-based heat-shrinkable film of the present invention preferably has an endothermic amount of 0.30 J / g or more and 0.95 J / g or less of non-reverse heat flow observed at 20°C to 60°C measured by a temperature-modulated differential scanning calorimeter (temperature-modulated DSC). If the endothermic amount is 0.95 J / g or less, the natural shrinkage rate can be reduced to 3.0% or less. A smaller endothermic amount is preferable because the natural shrinkage rate can be further reduced, but the technical lower limit of the present invention is 0.30 J / g. As for the upper limit, it is more preferably 0.90 J / g or less, and particularly preferably 0.85 J / g or less. This endothermic component will be described in detail below.
[0033] The present inventors have investigated a method for reducing the natural shrinkage over time of a polypropylene-based heat-shrinkable film obtained by stretching at a low temperature, and have found that the melting point and heat of fusion, which are related to the heat shrinkage rate that usually appears at high temperatures of 70° C. or higher, do not correlate with the natural shrinkage rate. In addition, since natural shrinkage occurs irreversibly over time at room temperature, which is considerably lower than the melting point of the resin, the inventors believe that the movement of amorphous molecular chains observed at room temperature or below is related to it.
[0034] Therefore, regarding the motion of amorphous molecular chains, in Non-Patent Document 1 "In-situ investigation on the structural evolution of mesomorphic isotactic polypropylene in a continuous heating process: Polymer 105 (2016) 133-143", p. 138, Fig. 9, it has been reported that in polypropylene that has been crystallized poorly by quenching, an endothermic peak derived from the rigid amorphous component appears at a temperature of 40 ° C to 60 ° C, which is higher than the glass transition temperature of normal polypropylene, 0 ° C. Non-Patent Document 1 does not describe the thermal shrinkage rate or natural shrinkage rate of the film, but in order to investigate the irreversible change of this rigid amorphous component, the inventors analyzed the non-reverse heat flow of the temperature-modulated DSC for the polypropylene-based heat-shrinkable film they are investigating. As a result, it was confirmed that there was an endothermic peak in the temperature range of 20 ° C to 60 ° C, and further found that the natural shrinkage rate and the amount of heat absorbed derived from this endothermic peak show a positive correlation. That is, the inventors have found that the natural shrinkage rate can be controlled by controlling the amount of heat absorbed in the range of 20° C. to 60° C., and have thus completed the present invention. The method for controlling the amount of heat absorbed will be described in the explanation of the film-forming method described later.
[0035] The polypropylene-based heat-shrinkable film of the present invention preferably has a refractive index (Ny) in the width direction measured by an Abbe refractometer of 1.490 or more and 1.530 or less, more preferably 1.500 or more and 1.520 or less. If Ny is 1.490 or less, the orientation is hardly advanced, so the required hot water shrinkage cannot be obtained, which is not preferable. Also, if Ny is 1.530 or more, the orientation is high, so that the number of high-melting crystals increases due to oriented crystallization, and the hot water shrinkage in the width direction decreases, which is not preferable.
[0036] The polypropylene-based heat-shrinkable film of the present invention must have a refractive index (Ny-Nx) measured by an Abbe refractometer, which is calculated by subtracting the refractive index (Nx) in the longitudinal direction from the refractive index (Ny) in the transverse direction, of 0.015 or more and 0.030 or less. More preferably, the refractive index is 0.016 or more and 0.028 or less, and particularly preferably, the refractive index is 0.018 or more and 0.026 or less. By stretching the film so that the balance between the refractive index in the longitudinal direction and the transverse direction is within the range, the required hot water shrinkage ratio in the longitudinal direction and the transverse direction can be obtained.
[0037] The present inventors have conducted extensive research into stretching a polypropylene-based raw material to obtain a high shrinkage ratio, and have found that by performing heat treatment and cooling under specified conditions before stretching in the width direction, crystal components in the low melting range of 70°C to 100°C are generated, and then stretching in the width direction at a low temperature from that state forms a structure having low melting crystals oriented in the stretching direction, thereby obtaining a high shrinkage ratio. Furthermore, the inventors have also studied a method for reducing the natural shrinkage ratio of the film after stretching by the above method, and have found a method for reducing the natural shrinkage ratio without impairing the shrinkage ratio obtained by stretching by performing a relaxation treatment (relaxation) on the stretched film under appropriate conditions. Based on these findings, the present inventors have arrived at the present invention. The specific method is described below.
[0038] When melt extruding the raw resin, it is preferable to dry the polypropylene-based resin raw material using a dryer such as a hopper dryer or a paddle dryer, or a vacuum dryer. After drying the polyolefin-based resin raw material in this way, it is melted at a temperature of 200 to 300°C and extruded into a film using an extruder. For such extrusion, any existing method such as a T-die method or a tubular method can be used.
[0039] An unstretched film can be obtained by quenching the sheet-like molten resin after extrusion to below 30° C. As a method for quenching the molten resin, a method can be suitably adopted in which the molten resin is cast from a die onto a rotating drum controlled at a low temperature by a cooling chiller or the like, and rapidly cooled and solidified to obtain a substantially unoriented resin sheet.
[0040] In the present invention, after obtaining the unstretched sheet as described above, the sheet may be stretched in the longitudinal direction from the viewpoint of improving the production speed and strength. When stretching in the longitudinal direction, the unstretched sheet preheated with a heating roll can be stretched by utilizing the speed difference between the rolls, as is done in general stretched film production. The roll temperature is preferably 50°C or more and 100°C or less. If the roll temperature is lower than 50°C, the film slips and the stretching is difficult to stabilize, which is not preferable. Also, if the roll temperature is higher than 100°C, the film is likely to fuse to the heating roll, and troubles such as the film wrapping around the roll are likely to occur, which is not preferable. A more preferable range of roll temperature is 55°C or more and 90°C or less. Also, the stretching ratio in the longitudinal direction is preferably 1.1 times or more and 2.0 times or less, and more preferably 1.2 times or more and 1.7 times or less. If the stretching ratio is more than 2.0 times, it is difficult to reduce the shrinkage in the longitudinal direction, and the distortion during heat treatment becomes large, which is likely to worsen the thickness unevenness, which is not preferable. Also, if the ratio is less than 1.1, the shrinkage rate in the longitudinal direction can be reduced, but there is almost no effect in terms of improving production speed.
[0041] Preferred conditions for stretching in the transverse direction and for the steps before and after the stretching will be described in detail below. (1) Heat treatment before transverse stretching In the production of the film of the present invention, it is preferable to heat-treat the film at a temperature of 70°C to 140°C for a time of 3.0 seconds to 50.0 seconds before stretching in the width direction. The heat treatment can be performed by providing a line for heat treatment using hot air or a ceramic heater while the film is being transported, or it can be performed in a tenter with both ends in the width direction held by clips before stretching in the width direction. By performing such heat treatment, crystalline components having a melting point in the low temperature range of 70°C to 100°C are selectively generated, and the crystalline components having a low melting point can remain even after stretching in the width direction, so that a heat-shrinkable film with a high shrinkage can be obtained. In addition, when stretching is performed in the longitudinal direction, this heat treatment also has the effect of reducing the shrinkage in the longitudinal direction.
[0042] If the temperature of the intermediate heat treatment exceeds 140°C, a crystalline component with a high melting point of 100°C or more is likely to be formed, and the shrinkage rate after stretching in the width direction is reduced, which is not preferable. On the other hand, if the temperature of the heat treatment is below 70°C, the formation of a crystalline component with a low melting point by the heat treatment hardly progresses, and the shrinkage rate during stretching in the width direction is likely to decrease, which is not preferable. In addition, when stretching in the longitudinal direction, the shrinkage rate in the longitudinal direction is high, which is not preferable. In addition, the lower limit of the heat treatment temperature is preferably 80°C or more, and more preferably 90°C or more. On the other hand, the upper limit of the heat treatment temperature is preferably 135°C or less, and more preferably 130°C or less. On the other hand, it is preferable to appropriately adjust the heat treatment time within the range of 1.0 second to 50.0 seconds depending on the raw material composition.
[0043] (2) Cooling after heat treatment and stretching in the width direction After the above-mentioned heat treatment, the film is preferably cooled to 70°C or less before stretching in the width direction. By performing cooling in this manner, it is possible to leave low-melting crystalline components. After such cooling, it is preferable to perform stretching in the width direction at a ratio of 2.5 to 10.0 times in a state where both ends in the width direction are held by clips in a tenter. The upper limit of the ratio of the transverse stretching is more preferably 9.0 times or less, and particularly preferably 8.0 times or less.
[0044] Furthermore, the stretching can be performed in two or more stages. That is, after stretching once in the width direction inside the tenter, a zone where stretching is not performed is provided, and then stretching is performed again in the width direction inside the tenter. The stretching ratio in the first stage is preferably 1.5 times or more and 7 times or less, and more preferably 2 times or more and 5.5 times or less. The stretching ratio in the second stage is preferably 1.5 times or more and 5 times or less, and more preferably 1.8 times or more and 3.5 times or less. The stretching ratios in each stage are adjusted within the above range so that the total stretching ratio is 2.5 times or more and 10.0 times or less. By performing the stretching in such a manner, it is possible to reduce breakage during stretching and also to easily reduce the increase in the natural shrinkage rate due to stretching.
[0045] The stretching temperature is preferably in the range of 50° C. to 100° C. If the stretching temperature is lower than 50° C., microvoids are generated during stretching, causing high haze and making the film more susceptible to breakage, which is undesirable, whereas if the temperature is higher than 100° C., low-melting-point crystalline components melt, causing not only a decrease in the shrinkage rate in the width direction but also large thickness unevenness in the width direction, which is undesirable. The lower limit of the temperature for stretching in the width direction is more preferably 55° C. or more, and particularly preferably 60° C. or more. The upper limit of the temperature for stretching in the transverse direction is more preferably 90° C. or less, and particularly preferably 85° C. or less.
[0046] (3) Relaxation treatment in the width direction (relaxation treatment) In addition, in producing a film by the transverse stretching method of the present invention, as described above, after stretching in the width direction, both ends of the film in the width direction are held by clips inside the tenter, and the tenter must be narrowed in the width direction to relax and shrink (relax) the film at a temperature of 60°C or higher and 100°C or lower for a time of 0.5 seconds to 20.0 seconds so that the relaxation rate calculated by Equation 2 is in the range of 13% to 40% of the length in the width direction. Relaxation rate = {(length before relaxation - length after relaxation) / length before relaxation} × 100 (%) Formula 2 If the temperature for performing the relaxation treatment is lower than 60°C, the film does not shrink sufficiently when relaxed, resulting in wrinkles, which is undesirable. If the temperature is higher than 100°C, the shrinkage rate decreases significantly, and the film will not shrink enough when used as a heat-shrinkable film, which is undesirable. The temperature for performing the relaxation treatment is more preferably 65°C to 95°C, and particularly preferably 70°C to 90°C. In addition, if the width direction length narrowed by the relaxation treatment is less than 13% of the length before the treatment, the heat absorption peak in the range of 20°C to 60°C observed by temperature modulated DSC cannot be sufficiently reduced, and the natural shrinkage rate increases, which is not preferable. In addition, if it is more than 40%, the 90°C shrinkage rate decreases and productivity decreases, which is not preferable. The relaxation treatment is preferably performed in the range of 15% to 35%, and particularly preferably 17% to 33%.
[0047] By carrying out such a relaxation treatment, it becomes possible to reduce the natural shrinkage rate while retaining the low melting point crystalline components of the final film and maintaining the shrinkage rate required for a heat shrinkable film. In addition, when the stretching in the width direction is carried out in two or more stages, the relaxation treatment can be carried out separately after each stretching. The relaxation treatment can be carried out by narrowing the tenter in the width direction, or by releasing the clips holding the film ends while applying heat near the tenter outlet and winding the film while shrinking it in the width direction.
[0048] In addition, only a specific one of the above means (1) to (3) is applied to the film in the width direction. However, it is believed that by combining all of the measures (1) to (3), it is possible to very efficiently improve heat shrinkability in the width direction, reduce the natural shrinkage rate, and achieve stable film-formability. EXAMPLES
[0049] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples and can be modified as appropriate without departing from the spirit of the present invention. The raw materials used in the examples and comparative examples, as well as the raw material compositions and film production conditions (stretching and heat treatment conditions, etc.) used in the examples and comparative examples are shown in Tables 1, 2 and 3. The resin raw materials PP1 to PP6, PE, COP, petroleum resin and amorphous PET in Table 1 are as follows: Resin raw material PP1: Polypropylene-butene random copolymer (manufactured by Mitsui Chemicals, Inc., product name "Tafmer XM7070", MFR = 7.0g / 10min, melting point 77℃, specific gravity 0.88) Resin raw material PP2: Polypropylene-butene random copolymer (manufactured by Mitsui Chemicals, Inc., product name "Tafmer XM7080", MFR = 7.0g / 10min, melting point 83℃, specific gravity 0.88) Resin raw material PP3: Polypropylene-ethylene random copolymer (Japan Polypropylene Corporation, product name "Novatec EG6D", MFR = 1.9g / 10min, melting point 145℃, specific gravity 0.90) Resin raw material PP4: Polypropylene-ethylene random copolymer (Japan Polypropylene Chemical Co., Ltd., product name "Wintec WFX6", MFR = 2.0g / 10min, melting point 125℃, specific gravity 0.90) Resin raw material PP5: Polypropylene (manufactured by Sumitomo Chemical Co., Ltd., product name "FS2011DG3", MFR = 2.5g / 10min, melting point 159℃, specific gravity 0.91) Resin raw material PP6: Polypropylene-ethylene random copolymer (Japan Polypropylene Corporation, Wintech WFX4T, MFR=7.0g / 10min, melting point 125℃, specific gravity 0.90) Resin raw material PE: Low density polyethylene resin (manufactured by Sumitomo Chemical Co., Ltd., product name "Excellen FX307", MFR = 3.2g / 10min, melting point 83℃, specific gravity 0.89) Resin raw material COP: Cyclic olefin resin (manufactured by Topas Advanced Polymers: product name "TOPAS9506F", MFR = 6.0g / 10min, glass transition temperature 65℃, specific gravity 1.01) Petroleum resin 1: Alicyclic hydrocarbon resin-based petroleum resin (manufactured by Arakawa Chemical Industries, Ltd.: product name "Alcon P-125", softening point 125°C, specific gravity 1.04) Amorphous PET: Neopentyl glycol copolymerized polyethylene terephthalate (30 mol% neopentyl glycol, intrinsic viscosity 0.72 dL / g, glass transition temperature 75°C) The MFR values shown are those at 230°C for polypropylene resins and cyclic olefin resins, and those at 190°C for polyethylene resins. The film was evaluated as follows.
[0050] [Tm (melting point)] Using a Shimadzu Corporation differential scanning calorimeter (model: DSC60), 5 mg of film was placed in an aluminum pan and heated from -40°C to 200°C at a heating rate of 10°C / min. The heat flow (unit: W / g) at each temperature was measured at sampling intervals of 0.5 seconds, and a heat flow curve was obtained by plotting the heat flow (negative direction is endothermic) on the vertical axis and the temperature (unit: °C) on the horizontal axis. A regression line was created for the heat flow curve between 55 and 60°C. The difference between the value on the regression line and the value on the heat flow curve was calculated for each temperature from 60°C to 175°C, starting from the low temperature side. The melting initiation temperature was determined as the temperature at which the difference first exceeded 0.001 W / g. Similarly, a regression line was created for the heat flow curve values from 175°C to 180°C. For the heat flows from 175°C to 60°C, the difference between the values on the regression line and the values on the heat flow curve was calculated in ascending order from the high temperature side. The melting end temperature was determined as the temperature at which the difference first exceeded 0.001 W / g. The straight line passing through the points on the heat flow curve at the melting start temperature and the melting end temperature was taken as the baseline. For the heat flows at each temperature from 70°C to 170°C, the difference was calculated by subtracting the value on the heat flow curve from the value on the baseline. Among the difference values at each temperature, the point where the value was greater than 0.02 W / g and was a maximum value for the temperature was taken as the melting peak of the heat flow curve, and the temperature of the melting peak was taken as the melting point.
[0051] [Heat absorption in non-reverse heat flow of temperature modulated DSC] Using a temperature modulated differential scanning calorimeter (TM DSC) "DSC250" (manufactured by TA instruments), 5 mg of the film was weighed into a T-ZERO pan, and in heat-only mode, the temperature was raised from -40°C to 200°C at an average heating rate of 2°C / min with a modulation period of 40 seconds, and the non-reverse heat flow was measured at sampling intervals of 0.1 seconds, and a non-reverse heat flow curve was obtained with the non-reverse heat flow (unit: W / g, negative direction is endothermic) on the vertical axis and the temperature (unit: °C) on the horizontal axis. For the non-reverse heat flow curve, a regression line was created from values between 18 and 20°C. For the non-reverse heat flow, the difference between the value on the regression line and the value on the non-reverse heat flow curve was calculated in order from the low temperature side in the range of 20°C to 60°C, and the temperature at which this value first became 0.0005 W / g or higher was defined as the endothermic onset temperature. Similarly, a regression line was created from the values on the non-reverse heat flow curve from 60° C. to 62° C. The difference between the values on the regression line and the values on the non-reverse heat flow curve was calculated from 60° C. to 20° C. The endothermic end temperature was determined as the temperature at which the difference first became 0.0005 W / g or more. The straight line connecting the points on the non-reverse heat flow curve at the endothermic start temperature and endothermic end temperature was used as the baseline, and the area enclosed by the non-reverse heat flow curve and the baseline was calculated to determine the endothermic amount of the peak (unit: J / g).
[0052] [Identification of α-olefin components] The type of α-olefin such as ethylene or butene in the propylene-α-olefin copolymer is determined by 13C NMR spectroscopy according to the method described on pages 615-617 of Polymer Analysis Handbook (published by Kinokuniya Shoten in 1995). It is also possible to determine by IR spectroscopy according to the method described on page 256 of the same book, section "(i) Random Copolymer."
[0053] [Heat shrinkage rate (hot water heat shrinkage rate)] The film was cut into a 10 cm x 10 cm square parallel to the unwinding direction of the roll (hereinafter, for the cut film, the unwinding direction of the roll before cutting is referred to as the longitudinal direction, and the direction perpendicular to the unwinding direction on the film surface is referred to as the width direction), and the film was immersed in warm water of a specified temperature ±0.5°C for 10 seconds under no load to allow it to shrink thermally. It was then immersed in water at 23°C ±0.5°C for 10 seconds and pulled out of the water, and the longitudinal and width dimensions of the film were measured and the thermal shrinkage percentage for each was calculated according to formula 1 above.
[0054] [Natural shrinkage rate] The film was cut into a 210 mm x 210 mm square parallel to the unwinding direction of the roll, and a 200 mm mark was drawn in each of the longitudinal and transverse directions of the cut sample. The sample was then left to stand for 672 hours in an atmosphere of 40°C and 65% RH for aging. The natural shrinkage rate (transverse direction) was calculated using the following formula 3. Natural shrinkage rate = {(gauge line length in width direction before aging - gauge line length in width direction after aging) / gauge line length in width direction before aging} x 100 (%) Formula 3
[0055] [Hayes] Measurement was performed using a haze meter (300A, manufactured by Nippon Denshoku Industries Co., Ltd.) in an atmosphere at 23° C. in accordance with JIS K 7105. The measurement was performed twice, and the average value was calculated.
[0056] [specific gravity] The specific gravity of the film was calculated from the ratio of the density of the film measured by a density gradient tube method in accordance with JIS K7112 to the density of water at a temperature of 23°C.
[0057] [Refractive index] Using an Atago Co., Ltd. Abbe Refractometer Model 4T, the sample films before shrinking were left in an atmosphere of 23±2°C and 65±5% RH for more than 2 hours, and then the refractive index (Nx, Ny) was measured in the longitudinal and transverse directions.
[0058] [Shrinkage finish] Label shrinkage distortion A cylindrical label (a label with the main shrinkage direction of the heat shrinkable film as the circumferential direction) was produced by overlapping both ends of a heat shrinkable film with a lattice pattern with 10 mm intervals in advance by 5 mm and thermally fusing it with an impulse sealer "HAKKO311" (manufactured by Hakkosha). A 500 ml PET bottle (body diameter 67 mm, minimum neck diameter 25 mm, product name "Jurokucha") was covered with the label and passed through a Fuji Astec Inc. steam tunnel (model: SH-1500-L) with a zone temperature of 85°C for 10.0 seconds to heat shrink the label and attach it to the bottle. Note that when attaching, the neck was adjusted so that the part with a diameter of 43 mm was at one end of the label. To evaluate the finish after shrinkage, the amount of deviation from the horizontal plane of the lattice pattern in the 360-degree direction of the attached label body, excluding the lattice including the fused part, was measured as distortion, and the maximum distortion was obtained. Evaluation was performed according to the following criteria. ◎: Maximum distortion less than 1.0mm ○: Maximum distortion 1.0mm or more and less than 2.0mm ×: Maximum distortion 2.0mm or more
[0059] [Wrinkles on label] The label was attached to a PET bottle under the same conditions as those for the shrinkage distortion of the label described above, and the occurrence of wrinkles was evaluated according to the following criteria. ◎: 0 wrinkles measuring 2mm or larger. ○: The number of wrinkles 2 mm or larger is 1 to 2. ×: 3 or more wrinkles measuring 2 mm or more.
[0060] [Evaluation of roll appearance after aging] (Appearance change after storage at 40℃ for 672 hours) The film was slit into a roll 300 mm wide and 300 m long and then wound up. The roll was placed in a temperature-controlled room with an atmosphere adjusted to 40°C and 65±10% RH. After storing for 672 hours, the roll was removed from the temperature-controlled room and 3 m of the film was unwound from the roll. The state of wrinkles was evaluated according to the following criteria. ◎: 0 wavy wrinkles measuring 1 cm or more. ○: The number of wavy wrinkles of 1 cm or more is 1 to 2. ×: 3 or more wavy wrinkles of 1 cm or more.
[0061] [Heat resistance blocking evaluation] Two pieces of film were cut into a 100mm x 100mm square, and the two pieces of film were overlapped with the corners offset by 45°, sandwiched between two 150mm x 150mm square aluminum plates with a thickness of 1mm, and heated for one minute in a hot air oven set at 80±0.5°C with a weight placed on top and a load of 500g applied. After that, the film was removed while still sandwiched between the aluminum plates, and cooled by immersing it in cold water at 23°C±0.5°C for 10 seconds, after which the blocking state of the overlapping films was evaluated according to the following criteria. ○: The films can be peeled off from each other and there is no blocking ×: Films are stuck together and blocking occurs
[0062] [Floating / sinking separation proper evaluation] The film was cut into a 100 mm x 100 mm square and placed in a cylindrical container with a bottom diameter of 130 mm, 2 L of water was added, and the temperature was adjusted to 23°C ± 2°C. The film was then sunk to the bottom, taking care to avoid any bubbles adhering to the container, and visually evaluated whether the film floated out of the water according to the following criteria. ○: The film floats up to the water surface ×: The film does not float to the water surface.
[0063] [Example 1] Polypropylene resins PP1 and PP3 were dry-blended in a weight ratio of 60 / 40 from the extruder, and SiO was added as a lubricant. 2 (Silisia 266 manufactured by Fuji Silysia Ltd.) was added at 500 ppm, melt extruded at 230°C, and quenched by winding it around a rotating metal roll cooled to 20°C to obtain an unstretched film (polypropylene resin sheet) with a thickness of 215 μm. The take-up speed of the unstretched film (rotation speed of the metal roll) was about 7.5 m / min.
[0064] Thereafter, the obtained unstretched film was heat-treated with hot air in a heat treatment zone provided on a conveying line in which a plurality of roll groups were arranged in series until the film temperature reached 100°C, and then air-cooled to 60°C and introduced into a tenter provided with a transverse stretching zone and a relaxation treatment zone arranged in series.
[0065] After preheating the film to a temperature of 60°C, the film was stretched 3.0 times in the width direction at 60°C in the first stage in the transverse stretching zone, and then stretched 2.2 times in the second stage at 60°C.Then, in the relaxation treatment zone, the film was relaxed by 20% at 75°C for 7 seconds to obtain a transverse uniaxially stretched film with a thickness of 40 μm.
[0066] The end of the film after the transverse uniaxial stretching as described above was slit and wound up on a paper tube to obtain a film roll of a transverse uniaxially stretched film (polypropylene-based heat-shrinkable film) with a width of 500 mm and a thickness of 40 μm wound up to a predetermined length. The properties of the obtained film were evaluated by the above-mentioned method. The evaluation results are shown in Table 2. As shown in Figure 1, two melting points were confirmed by DSC, the lower one being 93°C and the higher one being 145°C.
[0067] [Example 2] A film was produced in the same manner as in Example 1, except that the weight ratio of PP1 and PP3 in the polypropylene resins used was changed to 75 / 25, to obtain a uniaxially stretched transverse film having a thickness of 40 μm. The evaluation results are shown in Table 2.
[0068] [Example 3] The polypropylene resins used were changed to a weight ratio of PP1 and PP3 of 45 / 55, but film production was carried out in the same manner as in Example 1 to obtain a uniaxially stretched transverse film having a thickness of 40 μm. The evaluation results are shown in Table 2.
[0069] [Example 4] A film was produced in the same manner as in Example 1, except that the polypropylene resins used were changed to PP2 and PP3, and mixed in a weight ratio of 60 / 40, to obtain a uniaxially stretched transverse film having a thickness of 40 μm. The evaluation results are shown in Table 2.
[0070] [Example 5] A film was produced in the same manner as in Example 1, except that the polypropylene resins used were changed to PP1 and PP4, and mixed in a weight ratio of 60 / 40, to obtain a uniaxially stretched transverse film having a thickness of 40 μm. The evaluation results are shown in Table 2.
[0071] [Example 6] A film was produced in the same manner as in Example 1, except that the polypropylene resins used were changed to PP1 and PP5, and mixed in a weight ratio of 60 / 40, to obtain a transverse uniaxially stretched film having a thickness of 40 μm. The evaluation results are shown in Table 2.
[0072] [Example 7] A film was produced in the same manner as in Example 1, except that the heating temperature in the heat treatment zone was changed to 75° C., to obtain a transverse uniaxially stretched film having a thickness of 40 μm. The evaluation results are shown in Table 2.
[0073] [Example 8] A film was produced in the same manner as in Example 1, except that the heating temperature in the heat treatment zone was changed to 125° C., to obtain a transverse uniaxially stretched film having a thickness of 40 μm. The evaluation results are shown in Table 2.
[0074] [Example 9] The unstretched sheet obtained in the same manner as in Example 1, except that the take-up speed of the unstretched film (the rotation speed of the metal roll) was about 6.3 m / min and the thickness was adjusted to 258 μm, was introduced into a longitudinal stretching machine in which a plurality of roll groups were arranged in series, and the film was preheated on a preheating roll until the film temperature reached 60° C., and then stretched 1.2 times between a low-speed stretching roll set to a surface temperature of 60° C. and a high-speed stretching roll in which the temperature of the internal circulating water was set to 30° C. The speed of the low-speed roll (the speed of the film moving together with the low-speed roll) was adjusted to 6.3 m / min., and the speed of the high-speed roll (the speed of the film moving together with the high-speed roll) was adjusted to 7.5 m / min., to obtain a longitudinal uniaxially stretched film having a thickness of 215 μm. The obtained longitudinally uniaxially stretched film was subjected to heat treatment, stretching, and relaxation treatment in the same manner as in Example 1 to obtain a biaxially stretched film having a thickness of 40 μm. The evaluation results are shown in Table 2.
[0075] [Example 10] The unstretched sheet obtained in the same manner as in Example 1, except that the unstretched film was taken up at a take-up speed of about 4.2 m / min and the thickness was adjusted to 366 μm, was then stretched in the same manner as in Example 9, except that the speed of the low-speed roll in the longitudinal stretching machine was adjusted to 4.4 m / min. and the speed of the high-speed roll was adjusted to 7.5 m / min., changing the stretch ratio to 1.7 times, to obtain a biaxially stretched film having a thickness of 40 μm. The evaluation results are shown in Table 2.
[0076] [Example 11] An unstretched sheet having a thickness of 225 μm was produced under the same conditions as in Example 1, except that the discharge amount was changed, and the unstretched sheet obtained was heat-treated in the same manner as in Example 1 and introduced into a tenter. Except that the relaxation rate after stretching was set to 15%, a film was produced in the same manner as in Example 1, to obtain a transverse uniaxially stretched film having a thickness of 40 μm. The evaluation results are shown in Table 2.
[0077] [Example 12] Under the same conditions as in Example 1, only the discharge amount was changed to produce an unstretched sheet having a thickness of 225 μm, and the unstretched sheet obtained was heat-treated in the same manner as in Example 1 and introduced into a tenter, after which it was preheated until the film temperature reached 60° C., and then the first stage of stretching was performed in the transverse stretching zone at 60° C. and 3.0 times in the width direction, and then introduced into the relaxation treatment zone and relaxed at 60° C. for 5 seconds, and then further stretched at 60° C. for the second stage of 2.2 times, and then relaxed at 75° C. for 5 seconds in the relaxation treatment zone to obtain a transverse uniaxially stretched film having a thickness of 40 μm. Except for this, a film was produced in the same manner as in Example 1 to obtain a transverse uniaxially stretched film having a thickness of 40 μm. The evaluation results are shown in Table 2.
[0078] [Example 13] A 200 μm-thick unstretched sheet was produced under the same conditions as in Example 1, but only the discharge amount was changed, and the resulting unstretched sheet was heat-treated in the same manner as in Example 1 and introduced into a tenter. The first-stage stretching ratio was set to 6.6 times, and relaxation in the relaxation treatment zone was performed at 75° C. for 15 seconds at 25%, and no second-stage stretching was performed. Except for this, a 40 μm-thick transverse uniaxially stretched film was produced in the same manner as in Example 1. The evaluation results are shown in Table 2.
[0079] [Example 13] Under the same conditions as in Example 1, only the discharge amount was changed to produce an unstretched sheet with a thickness of 175 μm. The unstretched sheet obtained was heat-treated in the same manner as in Example 1 and introduced into a tenter, and then stretched in the width direction at a stretch ratio of 6.6 times. Thereafter, in a relaxation treatment zone set at 75 ° C., the clips holding the ends were released, and the ends were slit while being wound up as they were, and then wound up on a paper tube to obtain a uniaxially stretched film with a width of 500 mm and a thickness of 40 μm. The relaxation rate was calculated from the width of the raw roll at the exit of the tenter before slitting, and was 35%. The evaluation results are shown in Table 2.
[0080] [Example 14] Except for forming an unstretched sheet having a thickness of 110 μm under the same conditions as in Example 1 by changing only the discharge amount, a heat treatment, stretching, and relaxation treatment were performed in the same manner as in Example 1 to obtain a transverse uniaxially stretched film having a thickness of 20 μm. The evaluation results are shown in Table 2.
[0081] [Example 15] Except for forming an unstretched sheet having a thickness of 420 μm under the same conditions as in Example 1 by changing only the discharge amount, a heat treatment, stretching, and relaxation treatment were performed in the same manner as in Example 1 to obtain a transverse uniaxially stretched film having a thickness of 80 μm. The evaluation results are shown in Table 2.
[0082] [Comparative Example 1] A film was produced in the same manner as in Example 1, except that the polypropylene resin used was changed to PP3 alone, and a uniaxially stretched film having a thickness of 40 μm was obtained. The evaluation results are shown in Table 3. The melting point measured by DSC was only observed at 145° C., as shown in FIG. 1. Since no low-melting-point resin was used, whitening occurred due to voids during stretching, and the haze increased. In addition, since the shrinkage rate was low, the relaxation treatment could not be performed as set, and the film wrinkled during film production. Since the shrinkage rate of the obtained film was significantly insufficient, it was not practical to use it as a heat-shrinkable film.
[0083] [Comparative Example 2] A film was produced in the same manner as in Example 7, except that the polypropylene resin used was changed to PP1 alone, and a transverse uniaxially stretched film with a thickness of 40 μm was obtained. The evaluation results are shown in Table 3. Since no high melting point resin was used, the film melted and deformed, so it was not possible to measure the hot water shrinkage rate at 90°C. In addition, when the finish was evaluated, the film was fused to the PET bottle when heated, and wrinkles occurred at the fused portion. Blocking also occurred in the heat resistance blocking evaluation, and the film was unsuitable for practical use due to insufficient heat resistance.
[0084] [Comparative Example 3] An unstretched sheet having a thickness of 215 μm was formed in the same manner as in Example 1, except that the heating temperature in the heat treatment zone was changed to 60° C., and a transverse uniaxially stretched film having a thickness of 40 μm was obtained. The evaluation results are shown in Table 3. Because the heat treatment temperature was low, the melting peak was not formed at 100° C. or less, and the heat shrinkage rate of the obtained film was also insufficient. In the evaluation of the finished product, insufficient adhesion and the occurrence of wrinkles due to insufficient shrinkage were observed, and the film was poor in practical use as a heat shrinkable film.
[0085] [Comparative Example 4] An unstretched sheet having a thickness of 260 μm was produced in the same manner as in Example 1, and the unstretched sheet was introduced into a tenter. Except for changing the relaxation rate in each relaxation treatment zone to 0%, film production was performed in the same manner as in Example 1. The finished quality was good, but since no relaxation treatment was performed after stretching, the heat absorption observed at 20° C. to 60° C. in the temperature modulated DSC was large compared to Example 1, as shown in Table 3 and FIG. 2, and the natural shrinkage rate could not be reduced. Even when the film was unwound from the roll after aging, wavy wrinkles due to natural shrinkage were generated, and the film was poor in practical use in terms of ease of storage.
[0086] [Comparative Example 5] A 50 / 50 weight ratio dry blend of cyclic olefin resin COP1 and polyethylene resin PE1 was melt-extruded from an extruder at 230°C, and then rapidly cooled by winding it around a metal roll cooled to 20°C and rotating at about 7.5 m / min. to obtain an unstretched film having a thickness of 160 μm. The unstretched film obtained was then introduced into a tenter, preheated to 80°C, stretched 4 times at 80°C, and then cooled, slit as in Example 1, and wound around a paper tube to obtain a transverse uniaxially stretched film. The evaluation results are shown in Table 3. Although the natural shrinkage was relatively small because a cyclic olefin resin was used, the hot water shrinkage rate was insufficient and the shrink finish was not practically sufficient. The specific gravity was also larger than that of the film obtained in the examples.
[0087] [Comparative Example 6] Amorphous PET resin (neopentyl glycol copolymerized polyethylene terephthalate) was melt-extruded from an extruder at 260°C, and then wound around a metal roll cooled to 20°C and rotating at about 7.5 m / min. to rapidly cool the film, thereby obtaining an unstretched film having a thickness of 160 μm. The unstretched film obtained was then introduced into a tenter, preheated to 80°C, stretched 4 times at 80°C, and then cooled, slit and wound loosely in the same manner as in Example 1 to obtain a transverse uniaxially stretched film. The evaluation results are shown in Table 3. The shrink finish was good, but the film was not suitable for float-sink separation because the specific gravity was greater than 1.0.
[0088] [Comparative Example 7] Using a three-layer co-extrusion die and two extruders, an unstretched sheet having a thickness of 350 μm and a three-layer structure of ABA consisting of a surface layer A layer and a middle layer B layer was produced at a winding speed of about 7.5 m / min so that the ratio of the layer thickness of ABA was 1:8:1. At this time, PP6 resin was used for the A layer, and a mixture of PP4, PE1, and petroleum resin 1 in a ratio of 45 / 20 / 35 was used for the B layer. The obtained unstretched sheet was introduced into a tenter, heated to 80 ° C., and stretched 7 times to obtain a transverse uniaxially stretched film having a thickness of 50 μm. The end of the film after the transverse uniaxial stretching as described above was slit and wound on a paper tube to obtain a film roll in which a transverse uniaxially stretched film (polypropylene-based heat-shrinkable film) having a width of 500 mm and a thickness of 50 μm was wound up to a predetermined length. The properties of the obtained film were evaluated by the above-mentioned method. The evaluation results are shown in Table 3. The shrinkage finish was good, but the natural shrinkage rate was large, and the film that was unwound from the roll after aging had wavy wrinkles.
[0089] As is clear from Table 2, the films obtained in Examples 1 to 16 all had high shrinkage in the width direction and low shrinkage in the orthogonal longitudinal direction, and therefore showed good results in shrink finishing. In addition, by carrying out a relaxation treatment, the natural shrinkage rate could be reduced, and wrinkles were hardly observed after aging, so that the films were practically usable as heat-shrinkable films. In addition, since only polypropylene-based resins are used, the specific gravity is very small, and the films are suitable for floating-sinking separation with PET bottles. In contrast, the films obtained in Comparative Examples 1 to 7, as described in Table 3 and the above-mentioned items for each Comparative Example, did not have properties sufficient for practical use as heat-shrinkable films or suitable for floating-sinking separation.
[0090] [Table 1]
[0091] [Table 2A]
[0092] [Table 2B]
[0093] [Table 3] [Industrial Applicability]
[0094] The polypropylene-based heat-shrinkable film of the present invention has excellent shrinkage properties as described above, and therefore can be suitably used for packaging various items, including labels for PET bottles. In addition, since the specific gravity is less than 1.0, it is suitable for floating / sinking separation from PET bottles, and can contribute to the efficient recycling of PET bottles.
Claims
1. A polypropylene-based heat-shrinkable film for labels, which is a stretched film composed of a polypropylene-based resin composition and satisfies the following (1) to (6): (1) When the film is immersed in 90° C. hot water for 10 seconds, the hot water heat shrinkage is 40% or more and 80% or less in the width direction of the film. (2) When the film is immersed in 90° C. hot water for 10 seconds, the hot water heat shrinkage rate is −5% or more and 12% or less in the longitudinal direction of the film. (3) The specific gravity of the film is 0.87 or more and 0.95 or less. (4) The material has at least one melting peak temperature in the range of 70°C or higher and 100°C or lower, and at least one melting peak temperature in the range of more than 100°C and 170°C or lower, as measured by a differential scanning calorimeter. (5) The difference Ny-Nx between the refractive index in the width direction (Ny) and the refractive index in the longitudinal direction (Nx) is 0.015 or more and 0.030 or less. (6) The polypropylene-based heat-shrinkable film has a natural shrinkage rate in the width direction of 0.1% or more and 3.0% or less after aging for 672 hours under an atmosphere of 40° C. and 65% RH.
2. 2. The polypropylene-based heat-shrinkable film for labels according to claim 1, wherein the haze of the film is from 1% to 15%.
3. 3. The polypropylene-based heat-shrinkable film for labels according to claim 1 or 2, characterized in that the non-reverse heat flow measured by a temperature modulated scanning calorimeter has a peak in the range of 20°C or more and 60°C or less, and the heat absorption of the peak is 0.3 J / g or more and 0.95 J / g or less.
4. 4. The polypropylene-based heat-shrinkable film for labels according to claim 1, wherein the refractive index Ny in the width direction is 1.490 or more and 1.530 or less.
5. 5. The polypropylene-based heat-shrinkable film for labels according to claim 1, wherein the thickness of the polypropylene-based heat-shrinkable film is from 12 μm to 100 μm.
6. The polypropylene-based heat-shrinkable film for labels according to any one of claims 1 to 5, characterized in that the polypropylene-based resin composition constituting the polypropylene-based heat-shrinkable film contains ethylene or 1-butene as a copolymerization component.
Citation Information
Patent Citations
Controlling valve for farm working machinery of agricultural tractor
JP1981090103A
Film for heat resistant shrink label
JP1993309732A
Heat-shrinkable polypropylene film
JP1995256754A
Heat-shrinkable polypropylene-based film
JP2001294678A
Resin composition for heat-shrinkable polypropylene label and film using the same
JP2002060566A