Polyester film for surface protection of folding displays and its applications
A polyester film with specific mechanical properties and a hard coat layer addresses image distortion and productivity issues in foldable displays, providing clear images and improved portability.
Patent Information
- Application Number
- JP2023122165
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2017-03-02
- Filing Date
- 2023-07-27
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2038-02-14
AI Technical Summary
Conventional display surface protection films for foldable displays suffer from image distortion and poor mass productivity due to deformation at the folded portion, and existing thickness variation methods are inefficient.
A polyester film with a thickness of 10 to 75 μm and a 0.2% yield point strain of 2.6 to 5.0% in the bending direction, combined with a hard coat layer having a thickness of 1 to 50 μm and a pencil hardness of H or higher, is used to protect foldable displays, ensuring a bending radius of 5 mm or less.
The solution maintains mass productivity and prevents deformation, ensuring clear images without distortion at the folded portion, enhancing the functionality and portability of foldable displays.
Smart Images

Figure 0007568005000002 
Figure 0007568005000003 
Figure 0007568005000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyester film for surface protective film of a folding display, a hard coat film for surface protective film of a folding display, a folding display, and a mobile terminal device, and relates to a folding display and a mobile terminal device that are unlikely to suffer image distortion due to deformation of the film located on the surface even when repeatedly folded, and to a polyester film and a hard coat film for surface protective film of the folding display. [Background technology]
[0002] As mobile terminal devices become thinner and lighter, smartphones and other mobile terminal devices are becoming more and more popular. While mobile terminal devices are required to have a variety of functions, they are also required to be convenient. For this reason, the mobile terminal devices that are currently in use must be able to perform simple operations with one hand, and must have a small screen size of around 6 inches, since they are assumed to be stored in a pocket or the like.
[0003] On the other hand, tablet devices with screen sizes of 7 to 10 inches are highly functional and can be used not only for video content and music, but also for business purposes, drawing, reading, etc. However, they cannot be operated with one hand, are less portable, and have issues with convenience.
[0004] To achieve these goals, a method has been proposed of connecting multiple displays together to make them more compact (Patent Document 1), but this method has not become widespread because it leaves a bezel, which means the image is cut off and visibility is reduced.
[0005] In recent years, mobile terminals incorporating flexible displays and foldable displays have been proposed, which provide a large-screen display without interruption to the image and are convenient to carry around.
[0006] Here, in the case of conventional displays and mobile terminal devices that do not have a folding structure, the surface of the display can be protected by a non-flexible material such as glass, but in the case of a folding display, when a one-sided display is formed via a folding part, it is necessary to use a hard coat film that is flexible and can protect the surface. However, in a folding display, the part corresponding to a certain folding part is repeatedly folded, and therefore the film in that part deforms over time, causing problems such as distorting the image displayed on the display.
[0007] In view of this, a method has been proposed in which the film thickness is partially changed (see Patent Document 2), but this method has the problem of being poorly suited for mass production. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2010-228391 A [Patent Document 2] JP 2016-155124 A Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention seeks to solve the problems associated with conventional surface protection members for displays as described above, and aims to provide a foldable display that is easy to mass-produce and has no risk of image distortion at the folded portion after repeated folding, as well as a mobile terminal device equipped with such a foldable display, by providing a polyester film for surface protection films and a hard coat film for surface protection films for foldable displays. [Means for solving the problem]
[0010] That is, the present invention comprises the following: 1. A polyester film for surface protection of a folding display, characterized in that it is a polyester film having a thickness of 10 to 75 μm and has a 0.2% yield point strain in at least one of the longitudinal direction and the width direction of 2.6 to 5.0%. 2. The polyester film for surface protection of a folding display as described above in 1, characterized in that the 0.2% yield point strain in the bending direction is 2.6 to 5.0%. (Here, the bending direction refers to the direction perpendicular to the fold when folding the polyester film.) 3. The polyester film for surface protection of a folding display according to the above 1 or 2, characterized in that the intrinsic viscosity of the film is 0.60 to 1.0 dl / g. 4. A hard coat film for surface protection films of foldable displays, comprising a hard coat layer having a thickness of 1 to 50 μm on at least one side of the polyester film for surface protection films of foldable displays described in any one of 1 to 3 above. 5. A hard coat film for surface protection of a folding display, as described in 4 above, characterized in that the pencil hardness of the hard coat layer measured under a load of 750 g in accordance with JIS K5600-5-4:1999 is H or more. 6. A foldable display in which the hard coat film for surface protection of a foldable display described in 4 or 5 above is arranged as a surface protection film so that the hard coat layer is located on the surface, and the foldable display has a bending radius of 5 mm or less when folded. 7. The foldable display according to claim 6, characterized in that a single continuous hard coat film is disposed across the folding portion of the foldable display. 8. A mobile terminal device having the foldable display described in claim 6 or 7. Effect of the Invention
[0011] A folding display using the polyester film or hard coat film for surface protection film of a folding display of the present invention maintains mass productivity, and the polyester film or hard coat film does not deform after repeated folding, so that the image does not become distorted at the folded part of the display. A mobile terminal device equipped with such a folding display provides beautiful images, is highly functional, and has excellent convenience such as portability. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a schematic diagram showing the measurement points of the bending radius when folded in the present invention. [Diagram 2] FIG. 2 is a schematic diagram showing a bending direction of a polyester film for a surface protection film of a folding display according to the present invention. [Diagram 3] FIG. 2 is a schematic diagram for explaining the 0.2% proof stress point strain in the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] (display) The display in the present invention generally refers to a display device, and the types of displays include LCD, organic EL display, inorganic EL display, LED, FED, etc., but LCD, organic EL, and inorganic EL, which have a bendable structure, are preferred. In particular, organic EL and inorganic EL, which can reduce the layer structure, are particularly preferred, and organic EL, which has a wide color gamut, is even more preferred.
[0014] (Foldable display) The folding display is preferably a structure in which a single continuous display is folded in half when carried, thereby reducing the size by half and improving portability. At the same time, it is desirable that the display is thin and lightweight. Therefore, the bending radius of the folding display is preferably 5 mm or less, and more preferably 3 mm or less. If the bending radius is 5 mm or less, the display can be made thin when folded. The smaller the bending radius, the better, but it may be 0.1 mm or more, or 0.5 mm or more. Even if it is 1 mm or more, the practicality is sufficiently good compared to conventional displays that do not have a folding structure. The bending radius when folded is measured at the location of the symbol 11 in the schematic diagram of FIG. 1, and means the radius of the inside of the folded part when folded. The surface protective film described later may be located on the outside or inside of the folded display.
[0015] (Organic EL) The general configuration of an organic EL display consists of an organic EL layer consisting of an electrode / electron transport layer / light-emitting layer / hole transport layer / transparent electrode, a retardation plate to improve image quality, and a polarizing plate.
[0016] (Mobile terminal device with touch panel) When an organic EL display is used in a mobile terminal device having a touch panel, a touch panel module is placed on top of the organic EL display or between the organic EL layer and the retardation plate. In this case, if an impact is applied from above, the circuits of the organic EL and the touch panel may be broken, so a surface protection film is necessary, and it is preferable that a film placed on the front surface of the display as a surface protection film has a hard coat layer laminated on at least the front surface side of the display.
[0017] (Surface protection film for folding displays) As the surface protection film, any film having high light transmittance and low haze, such as a polyimide film, a polyester film, a polycarbonate film, an acrylic film, a triacetyl cellulose film, or a cycloolefin polymer film, can be used. Among these, polyimide films and polyester films having high impact resistance and sufficient pencil hardness are preferred, and polyester films which can be produced inexpensively are particularly preferred.
[0018] In the present invention, the polyester film may be a single-layer film made of one or more types of polyester resin, or when two or more types of polyester are used, it may be a multilayer film or an ultra-multilayer laminate film having a repeating structure.
[0019] Examples of polyester resins include polyester films made of polyethylene terephthalate, polybutylene terephthalate, polyethylene-2,6-naphthalate, or copolymers mainly composed of these resin components. Among these, stretched polyethylene terephthalate films are particularly preferred in terms of mechanical properties, heat resistance, transparency, cost, etc.
[0020] When a polyester copolymer is used for the polyester film, examples of the dicarboxylic acid component of the polyester include aliphatic dicarboxylic acids such as adipic acid and sebacic acid; aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and 2,6-naphthalenedicarboxylic acid; and polyfunctional carboxylic acids such as trimellitic acid and pyromellitic acid. Examples of the glycol component include fatty acid glycols such as ethylene glycol, diethylene glycol, 1,4-butanediol, propylene glycol, and neopentyl glycol, aromatic glycols such as p-xylene glycol, alicyclic glycols such as 1,4-cyclohexanedimethanol, and polyethylene glycols having an average molecular weight of 150 to 20,000. The mass ratio of the copolymerization components of the preferred copolymer is less than 20% by mass. When it is less than 20% by mass, the film strength, transparency, and heat resistance are maintained, which is preferable.
[0021] In addition, in the production of polyester film, the intrinsic viscosity of at least one type of resin pellet is preferably in the range of 0.60 to 1.0 dl / g. When the intrinsic viscosity is 0.60 dl / g or more, the impact resistance of the obtained film is improved, and disconnection of the internal circuit due to external impact is less likely to occur, which is preferable. In addition, it also contributes to small deformation when repeatedly bent, which is preferable. On the other hand, when the intrinsic viscosity is 1.00 dl / g or less, the increase in filtration pressure of the molten fluid is not too large, and film production can be easily and stably operated, which is preferable.
[0022] Regardless of whether the film has a single-layer structure or a laminated structure, the intrinsic viscosity of the film is preferably 0.60 dl / g or more. More preferably, it is 0.62 dl / g or more. Even more preferably, it is 0.68 dl / g or more. If it is 0.60 dl / g or more, fatigue resistance can be imparted and sufficient bending resistance effect can be obtained. On the other hand, a film having an intrinsic viscosity of 1.00 dl / g or less is preferable because it can be produced with good operability.
[0023] The thickness of the polyester film is preferably 10 to 75 μm, and more preferably 25 to 75 μm. When the thickness is 10 μm or more, an effect of improving pencil hardness is observed, and when the thickness is 75 μm or less, it is advantageous for weight reduction and is excellent in flexibility, processability, handleability, etc.
[0024] The surface of the polyester film of the present invention may be smooth or uneven, but since it is used for display surface covering, the deterioration of optical properties due to unevenness is not preferable. The haze is preferably 3% or less, more preferably 2% or less, and most preferably 1% or less. If the haze is 3% or less, the visibility of the image can be improved. The lower limit of the haze is preferably as small as possible, but it may be 0.1% or more, or 0.3% or more.
[0025] As mentioned above, in order to reduce haze, it is better for the unevenness of the film surface to be not too large. However, in order to provide a certain degree of slipperiness from the viewpoint of ease of handling, unevenness can be formed by blending a filler into the surface polyester resin layer or by coating a coat layer containing a filler during the film formation process.
[0026] The method of blending particles into the base film can be a known method. For example, it can be added at any stage of polyester production, but preferably it can be added as a slurry dispersed in ethylene glycol or the like at the stage of esterification, or after the completion of transesterification reaction and before the start of polycondensation reaction, and polycondensation reaction can be carried out. It can also be carried out by using a vented kneading extruder to blend the slurry of particles dispersed in ethylene glycol or water with polyester raw material, or by using a kneading extruder to blend dried particles with polyester raw material.
[0027] Among them, a method is preferred in which aggregated inorganic particles are homogeneously dispersed in a monomer liquid that will become a part of the polyester raw material, and then the filtered product is added to the remainder of the polyester raw material before, during, or after the esterification reaction. According to this method, since the monomer liquid has a low viscosity, homogeneous dispersion of the particles and highly accurate filtration of the slurry can be easily performed, and when added to the remainder of the raw material, the dispersibility of the particles is good and new aggregates are unlikely to be generated. From this viewpoint, it is particularly preferred to add to the remainder of the raw material in a low temperature state before the esterification reaction.
[0028] In addition, the number of protrusions on the film surface can be further reduced by a method in which, after obtaining a polyester containing particles in advance, the pellets are mixed and extruded with pellets not containing particles (master batch method).
[0029] The polyester film may contain various additives, such as antistatic agents, UV absorbers, and stabilizers, within a range that maintains the total light transmittance in a preferred range.
[0030] The total light transmittance of the polyester film is preferably 85% or more, and more preferably 87% or more. If the transmittance is 85% or more, visibility can be sufficiently ensured. Although it can be said that the higher the total light transmittance of the polyester film, the better, it may be 99% or less, or 97% or less.
[0031] The surface of the polyester film of the present invention may be subjected to a treatment for improving adhesion to a resin forming a hard coat layer or the like.
[0032] Examples of the surface treatment method include roughening treatment using sandblasting or solvent treatment, and oxidation treatment such as corona discharge treatment, electron beam irradiation treatment, plasma treatment, ozone or ultraviolet irradiation treatment, flame treatment, chromic acid treatment, or hot air treatment, and any of these methods can be used without any particular limitation.
[0033] In addition, the adhesion can be improved by an adhesion improving layer such as an easy-adhesion layer. The easy-adhesion layer can be made of any resin such as an acrylic resin, a polyester resin, a polyurethane resin, or a polyether resin, and can be formed by a general coating method, preferably a so-called in-line coating method.
[0034] The polyester film described above can be produced, for example, through a polymerization step in which inorganic particles are homogeneously dispersed in a monomer liquid that becomes a part of the polyester raw material, the dispersion is filtered, and then the dispersion is added to the remainder of the polyester raw material to polymerize the polyester, and a film formation step in which the polyester is melt-extruded through a filter into a sheet, which is cooled and stretched to form a base film.
[0035] Next, a method for producing a biaxially stretched polyester film will be described in detail using an example in which polyethylene terephthalate (hereinafter, referred to as PET) pellets are used as the raw material for the base film, but the present invention is not limited to this. In addition, the number of layers may be limited to a single layer or a multilayer structure. It is not something that can be achieved.
[0036] After mixing and drying PET pellets in a predetermined ratio, the mixture is fed to a known melt lamination extruder, extruded from a slit die into a sheet, and cooled and solidified on a casting roll to form an unstretched film. In the case of a single layer, one extruder is sufficient, but in the case of producing a film with a multilayer structure, two or more extruders, two or more manifolds or merging blocks (e.g., merging blocks having a rectangular merging portion) are used to laminate multiple film layers constituting each outermost layer, and a sheet of two or more layers is extruded from a die and cooled on a casting roll to form an unstretched film.
[0037] In this case, it is preferable to perform high-precision filtration to remove foreign matter contained in the resin at any location where the molten resin is kept at about 280° C. during melt extrusion. The filter material used for high-precision filtration of the molten resin is not particularly limited, but a filter material made of sintered stainless steel is preferable because it has excellent performance in removing aggregates and high-melting organic matter mainly composed of Si, Ti, Sb, Ge, and Cu.
[0038] Furthermore, the filtration particle size (initial filtration efficiency 95%) of the filter medium is preferably 20 μm or less, particularly preferably 15 μm or less. If the filtration particle size (initial filtration efficiency 95%) of the filter medium exceeds 20 μm, foreign matter with a size of 20 μm or more cannot be sufficiently removed. By using a filter medium with a filtration particle size (initial filtration efficiency 95%) of 20 μm or less to perform high-precision filtration of molten resin, productivity may decrease, but it is preferable to obtain a film with few protrusions due to coarse particles.
[0039] The 0.2% proof stress strain in at least one of the longitudinal direction (machine flow direction) and the transverse direction of the polyester film is preferably 2.6 to 5.0%, more preferably 3.0 to 5.0%. The 0.2% proof stress strain is a value used as a substitute for the yield point, whether or not a yield point appears in the stress-strain curve, and can be used as an index of the elastic region. Figure 3 shows a schematic diagram of a stress-strain curve for determining the 0.2% proof stress strain. Figure 3 shows an example of a case where a yield point does not appear. The 0.2% proof stress strain is determined by a normal tensile test. In the stress-strain curve, a parallel line is drawn from point Q, where the stress is 0 MPa and the strain is 0.2%, to OA, where Hooke's law holds true, and the point where it intersects with the stress-strain curve is the proof stress point P. The value of the strain at point H where a parallel line is drawn from the vertical axis and intersects with the strain axis is the 0.2% proof stress point strain. The 0.2% proof stress point strain can be obtained from the stress-strain curve as described above, but if the stress-strain curve is obtained using a tensile testing machine (Shimadzu AUTOGRAPH AG-X Plus 1kN), the calculated result of the 0.2% proof stress point strain can be obtained directly by setting the strain at 0.2% using Shimadzu AUTOGRAPH software TRAPEZIUM X.
[0040] When the 0.2% proof stress point strain is 2.6% or more, deformation due to strain occurring during folding is unlikely to occur, which is preferable. When it is 5.0% or less, good impact resistance is obtained, which is preferable. The 0.2% proof stress point strain in the bending direction of the polyester film is preferably 2.6 to 5.0%, and more preferably 3.0 to 5.0%. Here, the bending direction refers to the direction perpendicular to the folding part (reference number 21) assumed in the application of the surface protection film of a folding display, as shown by reference number 22 on the polyester film (reference number 2) in FIG. 2. The bending direction is not limited to either the longitudinal direction or the transverse direction of the film.
[0041] The 0.2% proof stress strain can be adjusted to fall within the above range by adjusting the stretch ratio, stretching temperature, heat setting temperature, polyester raw material, and the like.
[0042] The 0.2% proof stress point strain of the polyester film can be effectively adjusted by adjusting the stretching ratio. The stretching ratio of the unstretched polyester sheet in at least one of the longitudinal direction (machine flow direction) and the width direction is preferably 1.0 to 3.4 times, more preferably 1.0 to 3.0 times. By setting the stretching ratio to 1.0 to 3.4 times, the 0.2% proof stress point strain can be adjusted to a high range as described above, and deformation during repeated folding is small. The stretching direction is preferably the bending direction. The stretching temperature is preferably 80 to 130°C, more preferably 90 to 130°C. The heating method during stretching can be a conventionally known method such as a hot air heating method, a roll heating method, or an infrared heating method. By setting the stretching temperature to 80 to 130°C, thickness unevenness due to stretching at the above stretching ratio can be prevented.
[0043] From the viewpoint of the mechanical properties of the film, it is preferable that the stretching ratio in the direction perpendicular to the bending direction (direction of the folded part) is larger than that in the bending direction, and the stretching ratio in the direction perpendicular to the bending direction is, for example, 2.5 to 5.0. By setting the stretching ratio at 2.5 or more, stable productivity can be obtained, and by setting the stretching ratio at 5.0 or less, good impact resistance can be obtained.
[0044] The crystallinity of the polyester film is preferably 35 to 54%, more preferably 43 to 54%. By increasing the crystallinity, the 0.2% proof stress strain and impact resistance can be improved. In order to effectively increase the crystallinity, it is preferable to perform a heat treatment at 180 to 250°C after biaxial stretching. If the temperature is 180°C or higher, the crystallinity can be effectively increased, and if the temperature is 250°C or lower, there is no risk of the polyester film surface melting, and the appearance can be maintained good, which is preferable.
[0045] Specifically, for example, PET pellets are thoroughly vacuum-dried, then fed to an extruder, melt-extruded into a sheet at about 280°C, and cooled and solidified to form an unstretched PET sheet. The unstretched sheet obtained is stretched 1.0 to 3.4 times in the longitudinal direction with a roll heated to 80 to 130°C to obtain a uniaxially oriented PET film. Furthermore, the end of the film is held by a clip and introduced into a hot air zone heated to 80 to 180°C, dried, and then stretched 2.5 to 5.0 times in the width direction. Subsequently, the film is introduced into a heat treatment zone at 180 to 250°C, where heat treatment is performed for 1 to 60 seconds to complete the crystal orientation. During this heat treatment process, a relaxation treatment of 1 to 12% may be performed in the width direction or longitudinal direction as necessary.
[0046] (Hard coat layer) The polyester film that is placed on the surface of the foldable display to protect the display preferably has a hard coat layer on its surface. The hard coat layer is preferably placed on the display surface side of the polyester film and used in the display. The resin that forms the hard coat layer can be acrylic, siloxane, inorganic hybrid, urethane acrylate, polyester acrylate, epoxy, or other resins without any particular limitation. Two or more types of materials can be mixed and used, or particles such as inorganic filler or organic filler can be added.
[0047] (Film thickness) The thickness of the hard coat layer is preferably 1 to 50 μm, more preferably 1 to 40 μm. If it is thicker than 1 μm, it will be cured sufficiently and good pencil hardness will be obtained. Furthermore, by making the thickness 50 μm or less, curling due to cure shrinkage of the hard coat can be suppressed, and the handling properties of the film can be improved. It is more preferably 2 to 25 μm, particularly preferably 2 to 20 μm, and most preferably 3 to 15 μm.
[0048] (Application method) The hard coat layer can be applied by any method including, but not limited to, a Mayer bar, a gravure coater, a die coater, a knife coater, etc., and can be appropriately selected depending on the viscosity and film thickness.
[0049] (Curing conditions) The hard coat layer can be cured by energy rays such as ultraviolet rays and electron beams, or by heat, but curing methods using ultraviolet rays or electron beams are preferred in order to reduce damage to the film.
[0050] (Pencil hardness) The pencil hardness of the hard coat layer is preferably B or more, more preferably H or more, and particularly preferably 2H or more. If the hard coat layer has a pencil hardness of B or more, it is not easily scratched and does not reduce visibility. In general, the harder the hard coat layer has, the higher the pencil hardness is, but it may be 10H or less, 8H or less, or even 6H or less, and it can be used without any practical problems.
[0051] (Type of hard coat layer) The hard coat layer in the present invention may have other functions added thereto, so long as it can be used for the purpose of increasing the pencil hardness of the surface and protecting the display as described above.For example, hard coat layers with added functions such as antiglare layers, antiglare antireflection layers, antireflection layers, low reflection layers, and antistatic layers having a certain pencil hardness as described above are also preferably used in the present invention. EXAMPLES
[0052] Next, the effects of the present invention will be described using examples and comparative examples. First, the evaluation methods of the characteristic values used in the present invention will be described below.
[0053] (1) 0.2% yield point strain The film was cut into a strip of 10 mm width with a length of 140 mm in the measurement direction to obtain a sample, and a tensile test was performed at a tensile speed of 100 mm / min using a tensile tester (Shimadzu Corporation AUTOGRAPH AG-X Plus 1kN) to obtain a stress-strain curve. Then, the strain was set to 0.2% using Shimadzu Corporation's Autograph software TRAPEZIUM X, and the 0.2% yield point strain was calculated.
[0054] (2) Intrinsic viscosity The film or polyester resin was crushed and dried, and then dissolved in a mixed solvent of phenol / tetrachloroethane = 60 / 40 (mass ratio). After the solution was centrifuged to remove inorganic particles, the flow time of a solution with a concentration of 0.4 (g / dl) at 30°C and the flow time of the solvent alone were measured using an Ubbelohde viscometer, and the intrinsic viscosity was calculated from the time ratio using the Huggins formula and assuming that the Huggins constant is 0.38. In the case of a laminated film, the intrinsic viscosity of each layer alone was evaluated by scraping off the corresponding polyester layer of the film according to the laminate thickness.
[0055] (3) Crystallinity The density of the film sample was measured at three points. The average value was taken as the degree of crystallinity. The resin component was a mixture of completely amorphous and completely crystalline components, with a density as described below. Based on the assumption that the density of the sample is the sum of the masses of each component constituting the sample divided by the sum of the volumes of each component, the crystallinity (weight ratio) of each resin was estimated. The density of the sample was measured according to a method (density gradient tube method) compliant with JIS K-7112-1980. The density of each component alone was calculated using the following values (unit: g / cm3): Polyethylene terephthalate resin: completely amorphous 1.34, completely crystalline 1.46 Polyethylene naphthalate resin: completely amorphous 1.32, completely crystalline 1.41
[0056] (4) Flexibility A polyester film was cut into a size of 200 mm (bending direction) x 50 mm (orthogonal direction) to prepare a measurement sample. Spacers of each thickness were placed at the ends of two 5 mm thick glass plates to create a space, and the film was sandwiched between them and held for 10 seconds. Immediately after that, the film was exposed to fluorescent light, and the folded parts were observed, and the distance at which no folding marks were left was recorded. ○: The interval without folding marks was less than 6.5 mm. △: The gap where there were no folding marks was 6.5 mm or more and less than 7.0 mm ×: The interval where no folding marks were left was 7.0 mm or more.
[0057] (5) Repeated bending resistance A sample measuring 50 mm in the width direction and 100 mm in the machine direction was prepared. Using a no-load U-shaped stretch tester (Yuasa System Co., Ltd., DLDMLH-FS), the bending radius was set to 3 mm and the sample was bent 50,000 times at a speed of 1 time / second. During this process, the sample was fixed at positions 10 mm from both ends of the long side, and the bending area was 50 mm x 80 mm. After the bending process was completed, the sample was placed on a flat surface with the inside of the bend facing down and visually inspected. ○: No deformation of the sample or, even if there is deformation, the maximum lift when placed horizontally Less than 3mm in height. △: The sample is deformed and when placed horizontally, the maximum height of the rise is 3mm to 5mm less than. ×: The sample has a crease or the maximum height of the sample when placed horizontally is 5 mm or more.
[0058] (6)Pencil hardness The hard-coated polyester film thus produced was subjected to measurement in accordance with JIS K 5600-5-4:1999 at a load of 750 g and a speed of 0.5 mm / s.
[0059] (Coating solution 1 for forming hard coat layer) 0.1 parts by weight of a leveling agent (BYK307, 100% concentration, manufactured by BYK Japan) was added to 100 parts by weight of a hard coat material (Opstar (registered trademark) Z7503, manufactured by JSR Corporation, concentration 75%), and the mixture was diluted with methyl ethyl ketone to prepare hard coat coating solution 1 with a solid content concentration of 40% by weight.
[0060] (Coating solution 2 for forming hard coat layer) 95 parts by weight of a urethane acrylate hard coat agent (Beamset (registered trademark) 577, solids concentration 100%, manufactured by Arakawa Chemical Industries, Ltd.), 5 parts by weight of a photopolymerization initiator (Irgacure (registered trademark) 184, solids concentration 100%, manufactured by BASF Japan Ltd.), and 0.1 parts by weight of a leveling agent (BYK307, solids concentration 100%, manufactured by BYK Japan K.K.) were mixed and diluted with a solvent of toluene / MEK=1 / 1 to prepare coating solution 2 with a concentration of 40%.
[0061] (Preparation of polyethylene terephthalate pellets A) A continuous esterification reactor consisting of a three-stage complete mixing tank having an agitator, a partial condenser, a raw material inlet, and a product outlet was used as the esterification reactor, and the slurry was continuously fed to the first esterification reactor of the esterification reactor with TPA at 2 tons / hr, EG at 2 moles per mole of TPA, and antimony trioxide at an amount such that Sb atoms were 160 ppm relative to the produced PET, and reacted at normal pressure for an average residence time of 4 hours at 255°C. Next, the reaction product in the first esterification reactor was continuously taken out of the system and fed to the second esterification reactor, and EG distilled from the first esterification reactor was fed to the second esterification reactor at 8% by mass relative to the produced polymer (produced PET), and further, an EG solution containing magnesium acetate in an amount such that Mg atoms were 65 ppm relative to the produced PET and an EG solution containing TMPA in an amount such that P atoms were 20 ppm relative to the produced PET were added, and reacted at normal pressure for an average residence time of 1.5 hours at 260°C. Next, the reaction product in the second esterification reactor was continuously taken out of the system and fed to a third esterification reactor, and an EG solution containing TMPA in an amount such that the P atom was 20 ppm relative to the produced PET was added, and the reaction was carried out at normal pressure for an average residence time of 0.5 hours at 260°C. The esterification reaction product was continuously fed to a three-stage continuous polycondensation reaction apparatus to carry out polycondensation, and then filtered through a stainless steel sintered filter medium (nominal filtration accuracy: 90% cut of 5 μm particles) to obtain polyethylene terephthalate pellets A with an intrinsic viscosity of 0.62 dl / g.
[0062] (Preparation of polyethylene terephthalate pellets B) The polyethylene terephthalate pellets A were subjected to solid-phase polymerization at 220° C. for various times under a reduced pressure of 0.5 mmHg using a rotary vacuum polymerization apparatus to produce polyethylene terephthalate pellets B having an intrinsic viscosity of 0.72 dL / g.
[0063] (Preparation of polyethylene-2,6-naphthalate pellets C) 100 parts of dimethyl 2,6-naphthalenedicarboxylate, 60 parts of ethylene glycol, and 0.03 parts of manganese acetate tetrahydrate as an ester exchange catalyst were used to carry out an ester exchange reaction according to a conventional method, and then 0.042 parts of triethylphosphonoacetate were added to essentially terminate the ester exchange reaction. Next, 0.024 parts of antimony trioxide were added, and then polymerization reaction was carried out in a conventional manner under high temperature and high vacuum to obtain polyethylene-2,6-naphthalate (PEN) with an intrinsic viscosity of 0.60 dl / g. After that, the mixture was pre-dried at 150-160°C for 3 hours, and then solid-phase polymerization was carried out at 210°C, 13 kPa, and in a nitrogen gas atmosphere to obtain polyethylene-2,6-naphthalate pellets C with an intrinsic viscosity of 0.72 dl / g.
[0064] Example 1 The polyethylene terephthalate master pellet B was dried under reduced pressure (3 Torr) at 150°C for 8 hours, and then the polyethylene terephthalate pellet B was fed to the extruder and melted at 285°C. The polymer was filtered through a stainless steel sintered filter medium (nominal filtration accuracy 10μm particles 95% cut), extruded into a sheet from a die, and then contacted with a casting drum with a surface temperature of 30°C using an electrostatic casting method to cool and solidify, producing an unstretched film. The unstretched film was uniformly heated to 75°C using a heating roll, heated to 100°C with a non-contact heater, and roll-stretched (longitudinal stretching) 3.4 times. The obtained uniaxially stretched film was introduced into a tenter, heated to 140°C, stretched laterally 4.0 times, fixed in width, heat-treated at 240°C for 5 seconds, and further relaxed in the width direction at 210°C to obtain a polyethylene terephthalate film with a thickness of 50μm.
[0065] (Examples 2 to 6) A polyester film was obtained in the same manner as in Example 1 except that the stretching ratio and heat treatment temperature were changed to those shown in Table 1.
[0066] (Examples 7 and 8) A polyester film was obtained in the same manner as in Example 1 above, except that the thickness was changed to that shown in Table 1.
[0067] Example 9 A polyester film was obtained in the same manner as in Example 1 above, except that polyethylene-2,6-naphthalate pellets C were used as shown in Table 1 and the temperature was adjusted.
[0068] Example 10 A polyester film was obtained in the same manner as in Example 1, except that polyethylene terephthalate master pellets A were used instead.
[0069] Comparative Example 1 A polyester film was obtained in the same manner as in Example 1, except that the longitudinal stretching ratio was changed to 3.5 times.
[0070] (Comparative Examples 2 and 3) A polyester film was obtained in the same manner as in Example 1, except that the heat setting temperature was changed to that shown in Table 1.
[0071] One side of the polyester films obtained in the above Examples 1 to 10 and Comparative Examples 1 to 3 was coated with hard coat layer forming coating solution 1 using a Mayer bar so that the film thickness after drying would be 5.0 μm, and the film was dried at 80° C. for 1 minute, and then irradiated with ultraviolet light (high pressure mercury lamp, accumulated light amount 200 mJ / cm2) to obtain a hard coat film. In Example 11, the polyester film obtained in Example 1 was coated so that the film thickness after drying would be 10.0 μm, but the hard coat film was obtained in the same manner as in Example 1. In Example 12, the polyester film obtained in Example 1 was coated with hard coat layer forming coating solution 2, but the hard coat film was not coated. A hard coat film was obtained in the same manner as in Example 1.
[0072] These hard coat films were attached to an organic EL module via a 25 μm thick adhesive layer to create a smartphone-type foldable display that can be folded in half at the center of the entire display, which has a radius of 3 mm corresponding to the bending radius in FIG. 1. The hard coat film is arranged on the surface of one continuous display via the folding portion, and the hard coat layer is arranged so as to be located on the surface of the display. The hard coat films of each embodiment were satisfactory in terms of operation and visibility as a smartphone that can be folded in half at the center and carried around. On the other hand, the foldable displays using the hard coat films of each comparative example were not very preferable, as it seemed that image distortion occurred at the folding portion of the display as the frequency of use increased.
[0073] [Table 1] [Industrial Applicability]
[0074] According to a folding display using the polyester film or hard coat film for surface protection film of a folding display of the present invention, the polyester film or hard coat film located on the surface of the folding display does not deform after repeated folding while maintaining mass productivity, so that no image distortion occurs at the folded part of the display. A mobile terminal device equipped with a folding display using the polyester film or hard coat film of the present invention as a surface protection film provides beautiful images, is highly functional, and has excellent convenience such as portability. [Explanation of symbols]
[0075] 1: Foldable display 11: Bending radius 2: Polyester film for surface protection of folding displays 21: Folding section 22: Bending direction (direction perpendicular to the folding part) O: Origin A: The farthest point from O where Hooke's law holds P: A line parallel to the OA line drawn from Q intersects with the stress-strain curve Q: Stress 0 MPa, elongation (strain) 0.2% H: Draw a line parallel to the vertical axis from P and cross the horizontal axis (0.2% yield point strain (%)) σ0.2: Stress value of P (MPa)
Claims
1. The crystallinity is 35 to 54%, The total light transmittance is 85% or more and 99% or less, A polyester film for displays, characterized in that the 0.2% yield point strain in the machine direction is 2.6 to 5.0%.
2. A polyester film for displays as described in Claim 1, characterized in that the machine flow direction is a bending direction perpendicular to the folding portion when the polyester film is folded.
3. The polyester film for displays according to claim 1, characterized in that it has a thickness of 10 to 75 μm and an intrinsic viscosity of 0.60 to 1.0 dl / g.
4. A polyester film for displays as described in claim 1, characterized in that the haze is 0.1% or more and 3% or less.
5. In a no-load U-shaped stretch test in which the cable was bent 50,000 times at a bending radius of 3 mm and a speed of 1 time per second, after bending, the cable was placed horizontally on a flat surface with the inside of the bend facing down.
2. The polyester film for displays according to claim 1, which has a maximum lift height of less than 5 mm or is not deformed.
6. The polyester film for display according to any one of claims 1 to 5 has a hard coat layer having a thickness of 1 to 50 μm on at least one surface thereof, The pencil hardness of the hard coat layer measured under a load of 750 g in accordance with JIS K5600-5-4:1999 is H or more.
1. A hard coat film for displays, comprising:
7. A foldable display in which the hard coat film for a display according to claim 6 is arranged as a surface protective film so that the hard coat layer is positioned on a surface thereof, the foldable display has a bending radius of 5 mm or less when folded, A foldable display comprising a single continuous hard coat film disposed across the foldable portion of the display.
8. A mobile terminal device comprising the foldable display according to claim 7.
Citation Information
Patent Citations
Method of processing hard coat film, hard coat film and protective film
JP2010228391A
Transparent conductive substrate
JP2012156436A
Laminate, use thereof, and production method thereof
JP2016002764A
Laminate for organic el display device and organic el display device
JP2016126130A
Manufacturing method for foldable hard coating film
JP2016155124A