Urethane resin composition and laminate
The urethane resin composition with specific additives achieves stable foam retention and low-temperature flexibility, addressing the challenges of mechanical foaming in synthetic leather production, and is environmentally friendly.
Patent Information
- Application Number
- JP2023561553
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-11-18
- Filing Date
- 2022-11-10
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2042-11-10
AI Technical Summary
Existing urethane resin compositions for synthetic leather face challenges in forming films with excellent foam retention, crack resistance, and flexibility at low temperatures, particularly when mechanically foamed, due to issues like bubble instability and cracking during the foaming process.
A urethane resin composition containing a urethane resin with a nonionic group, water, polyoxyethylene alkyl ether, polyoxyethylene sorbitan fatty acid ester, and polyglycerol fatty acid ester, along with a film-forming aid, which enhances bubble retention and suppresses cracking, ensuring flexibility and texture even at low temperatures.
The composition forms films with superior foam retention, crack resistance, and flexibility at low temperatures, making it suitable for use in synthetic leather, particularly as a foam layer, while being environmentally friendly by eliminating the need for organic solvents.
Smart Images

Figure 0007568135000001 
Figure 0007568135000002 
Figure 0007568135000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a water-containing urethane resin composition. [Background technology]
[0002] Due to its mechanical strength and good texture, urethane resins are widely used in the manufacture of synthetic leather (including artificial leather). For this purpose, solvent-based urethane resins containing N,N-dimethylformamide (DMF) have been the mainstream. However, due to DMF regulations in Europe, strengthened VOC emission regulations in China and Taiwan, and DMF regulations by major apparel manufacturers, there is a demand to eliminate the use of DMF in the urethane resin compositions for each layer that makes up synthetic leather.
[0003] In this environment, polyurethane dispersions (PUDs), which are polyurethane resins dispersed in water, are beginning to be considered as an alternative raw material for the intermediate porous layer formed by wet coagulation of conventional solvent-based polyurethane resins. Various studies are being conducted on this alternative, using PUD foams to give the product the same texture as wet-formed membrane products.
[0004] As a method for obtaining the PUD foam, for example, the incorporation of microcapsules or mechanical foaming in which a gas such as carbon dioxide is dispersed in a PUD blend liquid has been considered (see, for example, Patent Document 1). However, in the method of incorporation of microcapsules, the texture of the obtained foam becomes poor, and there are problems with poor smoothness due to the expansion of the microcapsules. In addition, in the method of dispersing a gas, the air bubbles incorporated in the blend liquid disappear during the foam production process, making it difficult to control the bubble size, etc., and it has been difficult to stably obtain synthetic leather with a good texture.
[0005] In light of this, in recent years, mechanical foaming methods, in which PUD is mechanically stirred and foamed, have been considered as a simple way to obtain foam. However, the mechanical foaming method has problems, particularly in that the film can crack during drying, and bubbles can coalesce or disappear after the foaming process, resulting in unstable physical properties such as texture and flexibility at low temperatures. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2007-191810 A Summary of the Invention [Problem to be solved by the invention]
[0007] The problem to be solved by the present invention is to provide a water-containing urethane resin composition which is capable of forming a coating having excellent foam retention, crack resistance, texture, and flexibility at low temperatures even when mechanically foamed. [Means for solving the problem]
[0008] The present invention provides a urethane resin composition comprising a urethane resin (A) having a nonionic group, water (B), and a film-forming auxiliary (C) which is at least one selected from the group consisting of polyoxyethylene alkyl ether (c-1), polyoxyethylene sorbitan fatty acid ester (c-2), and polyglycerin fatty acid ester (c-3). The present invention also provides a laminate comprising at least a substrate (i) and a foamed layer (ii) formed from the urethane resin composition. Effect of the Invention
[0009] The urethane resin composition of the present invention contains water and is environmentally friendly. The urethane resin composition of the present invention can form a film having excellent foam retention, crack resistance, texture, and flexibility at low temperatures even when mechanically foamed. Therefore, the urethane resin composition of the present invention can be suitably used as a material for synthetic leather, and can be suitably used as a foam layer of synthetic leather in particular. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The urethane resin composition of the present invention contains a urethane resin (A) having a nonionic group, water (B), and a specific film-forming auxiliary (C).
[0011] In the present invention, it is essential to contain the specific film-forming auxiliary (C). It is presumed that the use of the specific film-forming auxiliary (C) improves foam retention in the system even after mechanical foaming of the urethane resin composition, thereby suppressing film cracking and providing a film with excellent texture and low-temperature flexibility.
[0012] As the film-forming auxiliary (C), it is essential to use one or more compounds selected from the group consisting of polyoxyethylene alkyl ethers (c-1), polyoxyethylene sorbitan fatty acid esters (c-2), and polyglycerin fatty acid esters (c-3).
[0013] As the polyoxyethylene alkyl ether (c-1), for example, polyoxyethylene lauryl ether, polyoxyethylene cetyl ether, polyoxyethylene stearyl ether, polyoxyethylene oleyl ether, etc. can be used. These compounds may be used alone or in combination of two or more. Among these, from the viewpoint of obtaining high hydrophilicity and more excellent foam retention, crack resistance, texture, and low-temperature flexibility, the number of moles added of the structure represented by the following formula (1) is preferably 30 or more, more preferably 50 or more, and even more preferably 80 or more. The upper limit is preferably 200 or less, more preferably 150 or less, and even more preferably 130 or less. The number of moles added of the structure represented by the following formula (1) in the (c-1) is preferably in the range of 30 to 200, more preferably 50 to 150, and even more preferably 80 to 130.
[0014] [ka]
[0015] As the polyoxyethylene sorbitan fatty acid ester (c-2), for example, polyoxyethylene sorbitan mono coconut oil fatty acid ester, polyoxyethylene sorbitan monopalmitate, polyoxyethylene sorbitan monostearate, polyoxyethylene sorbitan monolaurate, polyoxyethylene sorbitan monolaurate tristearate, polyoxyethylene sorbitan monolaurate monooleate, etc. can be used. These compounds may be used alone or in combination of two or more. Among these, the number of moles of the structure represented by formula (1) added is preferably 30 or more, more preferably 50 or more, and even more preferably 70 or more, from the viewpoint of high hydrophilicity and obtaining even more excellent foam retention, crack resistance, texture, and low-temperature flexibility. The upper limit is preferably 200 or less, more preferably 150 or less, and even more preferably 100 or less. The number of moles of the structure represented by the following formula (1) added in the above (c-2) is preferably in the range of 30 to 200, more preferably in the range of 50 to 150, and even more preferably in the range of 70 to 100.
[0016] Examples of the polyglycerol fatty acid ester (c-3) include polyglyceryl monocaprate, polyglyceryl monolaurate, polyglyceryl monomyristate, polyglyceryl monooleate, polyglyceryl monostearate, polyglyceryl dioleate, polyglyceryl distearate, and polyglyceryl pentaoleate. These compounds may be used alone or in combination of two or more. Among these, the HLB value (Hydrophilic-Lipophilic Balance) is preferably 5 or more, more preferably 10 or more, and even more preferably 14 or more, in terms of high hydrophilicity and excellent foam retention, crack resistance, texture, and low-temperature flexibility. The upper limit is preferably 25 or less, more preferably 20 or less, and even more preferably 18 or less. The HLB value of the polyglycerol fatty acid ester (c-3) is preferably in the range of 5 to 25, more preferably in the range of 10 to 20, and even more preferably in the range of 14 to 18.
[0017] The (c-1) to (c-3) may be used alone or in combination of two or more. The amount of the film-forming auxiliary (C) used is preferably in the range of 0.05 to 50 parts by mass, more preferably in the range of 0.1 to 20 parts by mass, based on 100 parts by mass of the urethane resin (A) (=solid content) described below.
[0018] The urethane resin (A) has a nonionic group, is dispersible in water, and does not require a crosslinking agent, so that excellent low-temperature flexibility can be obtained.
[0019] As a method for obtaining the urethane resin having a nonionic group, for example, a method using a compound having an oxyethylene structure as a raw material can be mentioned.
[0020] As the compound having an oxyethylene structure, for example, polyether polyols having an oxyethylene structure such as polyethylene glycol, polyoxyethylene polyoxypropylene glycol, polyoxyethylene polyoxytetramethylene glycol, and polyethylene glycol dimethyl ether can be used. These compounds may be used alone or in combination of two or more. Among these, it is preferable to use polyethylene glycol and / or polyethylene glycol dimethyl ether, since hydrophilicity can be controlled more easily.
[0021] The number average molecular weight of the compound having an oxyethylene structure is preferably in the range of 200 to 10,000, more preferably in the range of 300 to 3,000, still more preferably in the range of 300 to 2,000, and particularly preferably in the range of 300 to 1,000, in order to obtain even better emulsifiability and water dispersion stability. The number average molecular weight of the compound having an oxyethylene structure is a value measured by gel permeation column chromatography (GPC).
[0022] Specifically, the urethane resin (A) may be, for example, a reaction product of a chain extender (a1), a polyol (a2), a polyisocyanate (a3), and the compound having an oxyethylene structure.
[0023] The chain extender (a1) may have a molecular weight of less than 500 (preferably in the range of 50 to 450). Specifically, the chain extender (a1) may be ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, hexamethylene glycol, sucrose, methylene glycol, glycerin, sorbitol, bisphenol A, 4,4'-dihydroxydiphenyl, and 4,4'-dihydroxydiphenyl ether. , trimethylolpropane, and other hydroxyl group-containing chain extenders; ethylenediamine, 1,2-propanediamine, 1,6-hexamethylenediamine, piperazine, 2,5-dimethylpiperazine, isophoronediamine, 1,2-cyclohexanediamine, 1,3-cyclohexanediamine, 1,4-cyclohexanediamine, 4,4'-dicyclohexylmethanediamine, 3,3'-dimethyl-4,4'-dicyclohexylmethanediamine, 1,4-cyclohexanediamine, hydrazine, and other amino group-containing chain extenders can be used. These chain extenders may be used alone or in combination of two or more. The molecular weight of the chain extender (a1) is a value calculated from the chemical formula.
[0024] As the chain extender (a1), a chain extender having an amino group (hereinafter abbreviated as "amine-based chain extender") is preferred because it can easily extend the chain even at a relatively low temperature of 30 ° C. or less, and energy consumption during the reaction can be suppressed, and because the introduction of a urea group provides better mechanical strength, film-forming properties, foam retention, texture, low-temperature bending strength, and peel strength, and because the high solidification of the urethane resin (A) is easier to achieve. It is more preferable to use an amine-based chain extender having a molecular weight in the range of 30 to 250 because it provides better foam retention, emulsification, low-temperature bending strength, texture, and water dispersion stability. When two or more types of chain extenders are used in combination, the molecular weight indicates the average value, and the average value may be within the preferred molecular weight range.
[0025] The proportion of the chain extender (a1) used is more preferably in the range of 0.1 to 30 mass %, particularly preferably 0.5 to 10 mass %, of the total mass of the raw materials constituting the urethane resin (X), from the viewpoints of obtaining even better mechanical strength, film-forming properties, texture, peel strength, foam retention, emulsifiability, low-temperature flexibility, and water dispersion stability, and of facilitating high solids content of the urethane resin (A).
[0026] As the polyol (a2), for example, polyether polyol, polyester polyol, polyacrylic polyol, polycarbonate polyol, polybutadiene polyol, etc. can be used. These polyols may be used alone or in combination of two or more. As the polyol (a2), a compound other than the compound having the oxyethylene structure that imparts the nonionic group is used.
[0027] From the viewpoint of the mechanical strength of the resulting film, the number average molecular weight of the polyol (a2) is preferably in the range of 500 to 100,000, and more preferably in the range of 800 to 10,000. The number average molecular weight of the polyol (a2) is a value measured by gel permeation column chromatography (GPC).
[0028] The proportion of the polyol (a2) used is more preferably in the range of 40 to 90 mass %, particularly preferably 50 to 80 mass %, of the total mass of the raw materials constituting the urethane resin (A), in terms of obtaining even better mechanical strength.
[0029] Examples of the polyisocyanate (a3) include aromatic polyisocyanates such as phenylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, naphthalene diisocyanate, polymethylene polyphenyl polyisocyanate, and carbodiimidized diphenylmethane polyisocyanate; and aliphatic or alicyclic polyisocyanates such as hexamethylene diisocyanate, lysine diisocyanate, cyclohexane diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, xylylene diisocyanate, tetramethylxylylene diisocyanate, dimer acid diisocyanate, and norbornene diisocyanate. These polyisocyanates may be used alone or in combination of two or more.
[0030] The proportion of the polyisocyanate (a3) used is more preferably in the range of 5 to 40 mass %, particularly preferably 10 to 35 mass %, of the total mass of the raw materials constituting the urethane resin (A), in terms of obtaining even better mechanical strength.
[0031] The proportion of the compound having an oxyethylene structure used is preferably 5 mass % or less, more preferably 3 mass % or less, and even more preferably in the range of 0.25 to 3 mass %, based on the total mass of the raw materials constituting the urethane resin (A), in order to obtain even more excellent foam retention properties, emulsifiability, water dispersion stability, low-temperature flexibility, and film-forming properties.
[0032] The average particle size of the urethane resin (A) is preferably in the range of 0.01 to 1 μm, more preferably in the range of 0.05 to 0.9 μm, in order to obtain even better foam retention, surface smoothness, texture, low-temperature flexibility, and film-forming properties. The method for measuring the average particle size of the urethane resin (A) will be described in the Examples below.
[0033] The content of the urethane resin (A) in the urethane resin composition of the present invention is preferably 50 to 80% by mass, more preferably 50 to 70% by mass. Since the solid content of the urethane resin (A) in the aqueous dispersion is high, the retention is further improved even when foaming is performed by mechanical foaming, and the drying property of the urethane resin composition is improved, so that the crack resistance during and / or after drying is also excellent, and excellent texture and low-temperature flexibility can be obtained.
[0034] The water (B) used in the present invention may be ion-exchanged water, distilled water, etc. These waters may be used alone or in combination of two or more kinds.
[0035] Next, a method for producing the urethane resin (A) used in the present invention will be described.
[0036] The method for producing the urethane resin (A) used in the present invention comprises a step of reacting the polyol (a2), the polyisocyanate (a3), and the compound having an oxyethylene structure in the absence of a solvent to obtain a urethane prepolymer (i) having an isocyanate group (hereinafter abbreviated as the "prepolymer step"); then, dispersing the urethane prepolymer (i) in water (hereinafter abbreviated as the "emulsification step"); and thereafter, reacting with the chain extender (a1) to obtain the urethane resin (A) (hereinafter abbreviated as the "chain extension step").
[0037] The prepolymerization step is preferably carried out without a solvent. In the prior art, the prepolymerization step was generally carried out in an organic solvent such as methyl ethyl ketone or acetone, but a desolvation step for distilling off the organic solvent was required after the emulsification step, and this required several days of production at an actual production site. In addition, it is difficult to completely distill off the organic solvent in the desolvation step, and in many cases a small amount of organic solvent remains, making it difficult to fully comply with environmental requirements. On the other hand, by producing a prepolymer without a solvent, a urethane resin that is completely free of organic solvent can be obtained, and the production step can also be made more labor-saving.
[0038] In the prepolymer step, the molar ratio [isocyanate groups / (hydroxyl groups and amino groups)] of the sum of the hydroxyl groups in the polyol (a2) and the hydroxyl groups and amino groups in the compound having an oxyethylene structure to the isocyanate groups in the polyisocyanate (a3) is preferably in the range of 1.1 to 3, and more preferably in the range of 1.2 to 2, in order to obtain even better foam retention, low-temperature flexibility, crack resistance, surface smoothness, film-forming properties, texture, peel strength, and mechanical strength.
[0039] The reaction in the prepolymer step may be carried out, for example, at 50 to 120° C. for 1 to 10 hours.
[0040] The emulsification step can be carried out by using, for example, a reaction vessel equipped with an agitating blade; a kneading machine such as a kneader, a continuous kneader, a taper roll, a single-screw extruder, a twin-screw extruder, a triple-screw extruder, a universal mixer, a Plastomill, or a Bodeta-type kneader; a rotary dispersion mixer such as a homomixer, a static mixer, FILMICX, an Ebara Milder, a Clearmix, an Ultra-Turrax, a Cavitron, or a Biomixer; an ultrasonic dispersion device; or a device that has no moving parts and can mix by the flow of the fluid itself, such as an in-line mixer.
[0041] The emulsification step is preferably carried out at a temperature at which water does not evaporate, for example, in the range of 10 to 90° C. The emulsification step can be carried out using the same equipment as in the prepolymer step.
[0042] The chain extension step is a step of increasing the molecular weight of the urethane prepolymer (i) by reacting the isocyanate group of the urethane prepolymer (i) with the chain extender (a1) to obtain the urethane resin (A). From the viewpoint of productivity, the chain extension step is preferably performed at a temperature of 50° C. or less.
[0043] In the chain extension step, the molar ratio of the isocyanate groups in the urethane prepolymer (i) to the sum of the hydroxyl groups and amino groups in the chain extender (a1) [(hydroxyl groups and amino groups) / isocyanate groups] is preferably in the range of 0.8 to 1.1, and more preferably in the range of 0.9 to 1, in order to obtain even better low-temperature flexibility, crack resistance, film-forming properties, and mechanical strength.
[0044] The chain extension step can be carried out using the same equipment as the prepolymer step.
[0045] The urethane resin composition of the present invention contains the urethane resin (A), water (B), and film-forming auxiliary (C) as essential components, and may contain other additives as necessary.
[0046] Examples of the other additives include surfactants, crosslinking agents, emulsifiers, neutralizing agents, thickeners, urethanization catalysts, fillers, pigments, dyes, flame retardants, leveling agents, and antiblocking agents. These additives may be used alone or in combination of two or more. It is preferable that the urethane resin (A) is produced without substantially containing an organic solvent, but an organic solvent may be added as an additive.
[0047] As the surfactant, it is preferable to use a surfactant (D) having a hydrophobic portion having 10 or more carbon atoms, since this prevents the bubbles generated by mechanical foaming from disappearing and provides even better crack resistance and texture.
[0048] As the surfactant (D), for example, a surfactant represented by the following formula (2) can be used: fatty acid salt, succinate, sulfosuccinate, octadecylsulfosuccinate, sulfosuccinate, etc. These surfactants may be used alone or in combination of two or more.
[0049] [ka] (In the formula (2), R represents a linear or branched alkyl group having 10 to 20 carbon atoms, and X represents Na, K, NH4, morpholine, ethanolamine, or triethanolamine.)
[0050] As the surfactant (D), among the above-mentioned, it is preferable to use the surfactant represented by the above formula (2) in terms of obtaining even better foam retention, it is more preferable to use one having a linear alkyl group having 13 to 19 carbon atoms, and it is particularly preferable to use a stearate salt.
[0051] When the surfactant (D) is used, the amount used is preferably in the range of 0.01 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, per 100 mass of the urethane resin (A) (=solid content), in order to obtain even better foam retention.
[0052] Next, the laminate of the present invention will be described.
[0053] The laminate comprises at least a substrate (i) and a foam layer (ii) formed from the urethane resin composition.
[0054] Examples of the substrate (i) that can be used include fiber substrates such as nonwoven fabrics, woven fabrics, and knitted fabrics made of polyester fibers, polyethylene fibers, nylon fibers, acrylic fibers, polyurethane fibers, acetate fibers, rayon fibers, polylactic acid fibers, cotton, hemp, silk, wool, glass fibers, carbon fibers, and blends thereof; nonwoven fabrics impregnated with resins such as polyurethane resin; nonwoven fabrics further provided with a porous layer; and resin substrates such as thermoplastic urethane (TPU).
[0055] Next, a method for producing the laminate of the present invention will be described.
[0056] The method for producing the laminate includes, for example, (X) A method in which the urethane resin composition is foamed to obtain a foamed liquid, the foamed liquid is applied onto a release paper, dried, and then laminated to the substrate (i); (Y) A method in which the urethane resin composition is foamed to obtain a foamed liquid, the foamed liquid is applied onto a surface layer prepared on a release paper, the surface layer is dried, and the surface layer is laminated to the substrate (i); (Z) A method in which the urethane resin composition is foamed to obtain a foamed liquid, the foamed liquid is applied to the substrate (i), dried, and, if necessary, a surface layer (iii) prepared on a release paper is laminated thereon.
[0057] Examples of the method for foaming the urethane resin composition to obtain a foamed liquid include manual stirring and mechanical foaming using a mixer such as a mechanical mixer. Among these, the method using a mixer is preferred since the foamed liquid can be easily obtained. When a mixer is used, for example, a method of stirring at 500 to 3,000 rpm for 10 seconds to 10 minutes can be mentioned. In this case, in order to obtain a foamed layer (ii) having a good texture, it is preferable to make the volume 1.3 to 7 times, and more preferably 1.2 to 2 times, before and after foaming.
[0058] The obtained foamed liquid can be applied to the substrate (i) or the like by using, for example, a roll coater, a knife coater, a comma coater, an applicator, or the like.
[0059] The coating may be dried, for example, at a temperature of 60 to 130° C. for 30 seconds to 10 minutes.
[0060] The foamed layer (ii) obtained by the above method has a thickness of, for example, 5 to 300 μm.
[0061] The density of the foamed layer (ii) is preferably 200 to 1,000 kg / m from the viewpoint of obtaining a more excellent texture. 3 is preferably 400 to 800 kg / m 3 The density of the foamed layer (ii) is calculated by subtracting the weight of the base material (i) per 10 cm square from the weight of the laminate per 10 cm square, and dividing the result by the thickness of the foamed layer (ii).
[0062] The surface layer (iii) can be formed by a known method using a known material, and for example, a solvent-based urethane resin, a water-based urethane resin, a silicone resin, a polypropylene resin, a polyester resin, etc. can be used. When a soft texture, heat resistance, and hydrolysis resistance are important, it is preferable to use a polycarbonate-based urethane resin. In addition, in order to reduce DMF in an environmentally friendly manner, it is more preferable to use a water-based polycarbonate-based urethane resin.
[0063] If necessary, a surface treatment layer (iv) may be further provided on the surface layer (iii) for the purpose of improving scratch resistance, imparting gloss, etc. The surface treatment layer (iv) may be formed from a known material by a known method.
[0064] As described above, the urethane resin composition of the present invention contains water and is environmentally friendly. In addition, the urethane resin composition of the present invention can form a film having excellent foam retention, crack resistance, texture, and flexibility at low temperatures even when mechanically foamed. Therefore, the urethane resin composition of the present invention can be suitably used as a material for synthetic leather, and can be suitably used in particular as a foam layer of synthetic leather. EXAMPLES
[0065] The present invention will now be described in more detail with reference to examples.
[0066] [Synthesis Example 1] Preparation of urethane resin (A-1) composition In the presence of 0.1 part by mass of stannous octoate, 1,000 parts by mass of polyether polyol ("PTMG2000" manufactured by Mitsubishi Chemical Corporation, number average molecular weight: 2,000), 38 parts by mass of polyethylene glycol ("PEG600" manufactured by NOF Corporation, number average molecular weight: 600), and 262 parts by mass of dicyclohexylmethane diisocyanate (HMDI) were reacted at 100°C until the NCO% reached 2.8%, to obtain a urethane prepolymer. The urethane prepolymer heated to 70°C, 65 parts by mass of a 20% aqueous solution of emulsifier sodium dodecylbenzenesulfonate ("Neogen S-20F" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and 948 parts by mass of water were stirred and mixed in a homomixer to obtain an emulsion. Immediately after that, a water-diluted solution of isophoronediamine (IPDA) having an amino group content equivalent to the molar amount of NCO groups was added to extend the chain, and finally a urethane resin (A-1) composition with a urethane resin (A-1) content of 58% by mass was obtained.
[0067] [Synthesis Example 2] Preparation of urethane resin (A-2) composition In the presence of 0.1 part by mass of stannous octylate, 1,000 parts by mass of polycarbonate polyol (made from 1,6-hexanediol, number average molecular weight: 2,000), 18 parts by mass of PEG600, and 262 parts by mass of HMDI were reacted at 100°C until the NCO% reached 3.1% by mass, to obtain a urethane prepolymer. The urethane prepolymer heated to 70°C, 64 parts by mass of an emulsifier, a 20% aqueous solution of sodium dodecylbenzenesulfonate ("Neogen S-20F" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), and 811 parts by mass of water were stirred and mixed in a homomixer to obtain an emulsion. Immediately thereafter, a water-diluted solution of IPDA having an amino group content equivalent to 95% of the NCO groups was added to extend the chain, and finally a urethane resin (A-2) composition having a urethane resin (A-2) content of 60% by mass was obtained.
[0068] [Example 1] 100 g of the urethane resin (A-1) composition obtained in Synthesis Example 1, 2.0 g of a thickener "Borch Gel ALA" (manufactured by Borchers), 3.0 g of ammonium stearate, and 3.0 g of polyoxyethylene lauryl ether ("Nonion K-2100W" manufactured by NOF Corporation) were stirred at 2,000 rpm in a mechanical mixer to incorporate air and prepare a blended liquid having a volume of 150% of the initial volume. This was coated onto release paper and dried at 80°C for 3 minutes to obtain a 300μm thick urethane foam layer, which was then bonded to a nonwoven fabric to obtain synthetic leather.
[0069] [Example 2] 100 g of the urethane resin (A-1) composition obtained in Synthesis Example 1, 2.0 g of a thickener "Borch Gel ALA" (manufactured by Borchers), 3.0 g of ammonium stearate, and 3.0 g of polyoxyethylene sorbitan monolaurate ("Nonion LT-280" manufactured by NOF Corporation) were stirred at 2,000 rpm in a mechanical mixer to incorporate air and prepare a blended liquid having a volume of 150% of the initial volume. This was coated onto release paper and dried at 80°C for 3 minutes to obtain a 300μm thick urethane foam layer, which was then bonded to a nonwoven fabric to obtain synthetic leather.
[0070] [Example 3] 100 g of the urethane resin (A-2) composition obtained in Synthesis Example 2, 2.0 g of a thickener "Borch Gel ALA" (manufactured by Borchers), 3.0 g of ammonium stearate, and 3.0 g of polyglyceryl monolaurate ("Sunfact M12J" manufactured by Taiyo Kagaku Co., Ltd.) were stirred at 2,000 rpm in a mechanical mixer to incorporate air and prepare a blended liquid having a volume of 150% of the initial volume. This was coated onto release paper and dried at 80°C for 3 minutes to obtain a 300μm thick urethane foam layer, which was then bonded to a nonwoven fabric to obtain synthetic leather.
[0071] [Comparative Example 1] 100 g of anionic water-based urethane resin (DIC Corporation, "Hydran WLS-120AR"), 2.0 g of thickener "Borch Gel ALA" (Borchers), 3.0 g of ammonium stearate, 3.0 g of polyoxyethylene lauryl ether (NOF Corporation, "Nonion K-2100W"), and 4.0 g of crosslinker (Nisshinbo Chemical Inc., "Carbodilite SV-02") were stirred at 2,000 rpm in a mechanical mixer to incorporate air and prepare a mixed liquid with a volume of 150% of the initial volume. This was coated onto release paper and dried at 80°C for 3 minutes to obtain a 300μm thick urethane foam layer, which was then bonded to a nonwoven fabric to obtain synthetic leather.
[0072] [Comparative Example 2] 100 g of the urethane resin (A-1) composition obtained in Synthesis Example 1, 2.0 g of the thickener "Borch Gel ALA" (manufactured by Borchers), and 3.0 g of ammonium stearate were stirred at 2,000 rpm in a mechanical mixer to prepare a mixture having a volume of 150% of the initial volume by incorporating air. This was coated onto release paper and dried at 80°C for 3 minutes to obtain a 300μm thick urethane foam layer, which was then bonded to a nonwoven fabric to obtain synthetic leather.
[0073] [Method of measuring number average molecular weight, etc.] The number average molecular weights of the polyols and the like used in the Synthesis Examples and Comparative Synthesis Examples are values measured by gel permeation column chromatography (GPC) under the following conditions.
[0074] Measurement equipment: High-speed GPC equipment (Tosoh Corporation "HLC-8220GPC") Column: The following columns manufactured by Tosoh Corporation were used, connected in series. "TSKgel G5000" (7.8mm I.D. x 30cm) x 1 "TSKgel G4000" (7.8mm I.D. x 30cm) x 1 "TSKgel G3000" (7.8mm I.D. x 30cm) x 1 "TSKgel G2000" (7.8mmI.D. x 30cm) x 1 Detector: RI (differential refractometer) Column temperature: 40℃ Eluent: tetrahydrofuran (THF) Flow rate: 1.0mL / min Injection volume: 100 μL (sample concentration 0.4% by mass in tetrahydrofuran solution) Standard sample: A calibration curve was prepared using the following standard polystyrene.
[0075] (Standard polystyrene) "TSKgel Standard Polystyrene A-500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-1000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-2500" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene A-5000" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-1" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-2" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-4" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-10" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-20" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-40" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-80" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-128" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-288" manufactured by Tosoh Corporation "TSKgel Standard Polystyrene F-550" manufactured by Tosoh Corporation
[0076] [Method for measuring the average particle size of urethane resin (A)] The urethane resin compositions obtained in the examples and comparative examples were measured for average particle size using a laser diffraction / scattering type particle size distribution analyzer ("LA-910" manufactured by Horiba, Ltd.) with water as a dispersion liquid, a relative refractive index of 1.10, and an area as the particle size standard.
[0077] [Method for evaluating foam retention] In the examples and comparative examples, the foamed liquid was observed with a scanning electron microscope (SEM) before and after being left to stand for 2 hours after preparation, and the shape of the foam was confirmed and evaluated as follows. "Good": There is little change in bubble size, and little change in bubble volume and density. "X": The size of the bubbles has become very large, or the bubbles have disappeared and the density has increased.
[0078] [Crack resistance evaluation method] The appearance of the synthetic leathers obtained in the Examples and Comparative Examples was observed to check for the presence or absence of cracks. Those without cracks were rated as "good", and those with confirmed cracks were rated as "poor".
[0079] [How to evaluate texture] The synthetic leathers obtained in the Examples and Comparative Examples were touched with hands and evaluated as follows. "〇": Flexible and resilient "X": Less flexible and harder.
[0080] [Method of measuring low temperature flexibility] The synthetic leathers obtained in the Examples and Comparative Examples were subjected to a bending test (-35°C, 100 times / min) using a flexometer ("Flexometer with Low Temperature Bath" manufactured by Yasuda Seiki Seisakusho Co., Ltd.) to measure the number of times the synthetic leather was bent until cracks appeared on the surface of the synthetic leather, and evaluated as follows. "○": 10,000 times or more "×": Less than 10,000 times
[0081] [Table 1]
[0082] It was found that the urethane resin compositions of Examples 1 to 3 of the present invention gave synthetic leathers having excellent foam retention, crack resistance, texture, and low-temperature flexibility.
[0083] On the other hand, in Comparative Example 1, an anionic group-containing urethane resin was used instead of the nonionic group-containing urethane resin (A), but the low-temperature flexibility was poor.
[0084] Comparative Example 2 is an embodiment in which the film-forming auxiliary (C) was not used, and the foam retention, crack resistance, and feel were all poor.
Claims
1. A urethane resin composition comprising a urethane resin having a nonionic group (A), water (B), and a film-forming auxiliary (C) which is at least one selected from the group consisting of polyoxyethylene alkyl ethers (c-1), polyoxyethylene sorbitan fatty acid esters (c-2), and polyglycerin fatty acid esters (c-3), The urethane resin (A) contains, as essential raw materials, a chain extender (a1), a polyol (a2), a polyisocyanate (a3), and a compound having an oxyethylene structure, The polyol (a2) contains a polycarbonate polyol containing 1,6-hexanediol as an essential raw material, A urethane resin composition, characterized in that the content of the compound having an oxyethylene structure is in the range of 0.25 to 3 mass % based on the total mass of the raw materials for the urethane resin (A).
2. The urethane resin composition according to claim 1, wherein the number of moles of the structure represented by the following formula (1) added in the polyoxyethylene alkyl ether (c-1) is 30 or more: [Formula 1]
3. 3. The urethane resin composition according to claim 2, wherein the number of moles of the structure represented by the formula (1) added in the polyoxyethylene sorbitan fatty acid ester (c-2) is 30 or more.
4. The urethane resin composition according to any one of claims 1 to 3, wherein the polyglycerol fatty acid ester (c-3) has an HLB value of 5 or more.
5. The urethane resin composition according to any one of claims 1 to 4, further comprising a surfactant (D) having a hydrophobic moiety having 10 or more carbon atoms.
6. 6. The urethane resin composition according to claim 5, wherein the surfactant (D) is a stearate.
7. A laminate comprising at least a substrate (i) and a foamed layer (ii) formed from the urethane resin composition according to any one of claims 1 to 6.
8. 8. The laminate according to claim 7, wherein the foam layer (ii) is formed by mechanically foaming the urethane resin composition.
Citation Information
Patent Citations
Aqueous urethane resin composition for forming porous layer
JP2000297211A
Highly foamed fabric having polyurethane microporous membrane, and method for producing the same
JP2007191810A
Urethane resin composition and layered product
WO2020044894A1
Foam sheet and synthetic leather
WO2021084953A1