Sintered body, method for manufacturing sintered body, semiconductor manufacturing apparatus, and method for manufacturing semiconductor manufacturing apparatus
A high-density, high-hardness Y5O4F7 sintered body addresses corrosion and plasma resistance issues in semiconductor manufacturing equipment, reducing particle generation and enhancing equipment reliability.
Patent Information
- Application Number
- JP2020194856
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-25
- Publication Date
- 2024-10-16
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Semiconductor manufacturing equipment faces challenges with corrosion and particle generation due to halogen-based etching gases, and existing materials like Y2O3 lack sufficient hardness and plasma resistance, leading to scratches and abnormal discharge.
A high-density and high-hardness Y5O4F7 sintered body with a relative density of 97.0% or more and Vickers hardness of 2.4 GPa or more, manufactured through methods such as pressureless sintering and hot pressing, with optional HIP treatment, to enhance corrosion and plasma resistance.
The Y5O4F7 sintered body improves corrosion resistance and reduces particle generation, allowing for better plasma resistance and easier detection of abnormalities in semiconductor manufacturing equipment.
Smart Images

Figure 0007568489000001 
Figure 0007568489000002 
Figure 0007568489000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a sintered body, a method for manufacturing the sintered body, a semiconductor manufacturing apparatus, and a method for manufacturing the semiconductor manufacturing apparatus, and more particularly to a yttrium oxide fluoride (Y fluoride) for a member that comes into contact with plasma or radicals containing halogen gas in, for example, an etching apparatus and a chemical vapor deposition apparatus used in a semiconductor manufacturing process. 5 O 4 F 7 ) regarding materials. [Background technology]
[0002] As semiconductors become finer, there is a strong demand for low-contamination manufacturing processes. The impact of particles generated by dust in semiconductor manufacturing equipment, especially plasma etching equipment, is becoming a serious problem. Particles can be generated when halogen-based etching gas corrodes the inner walls and internal parts of a chamber. For this reason, corrosion resistance is required for the components used in semiconductor manufacturing equipment. Until now, alumina has been used as a corrosion-resistant material. Recently, Y, which has better corrosion resistance, has been used. 2 O 3 Technologies using yttrium oxide such as those mentioned above are becoming more and more practical.
[0003] In Patent Document 1 and Non-Patent Document 1, Y is used as a corrosion-resistant material. 5 O 4 F 7 Patent Document 1 and Non-Patent Document 1 disclose that a dense sintered body having a density of 99.0% or more can be obtained. [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] “Fabrication of dense yttrium oxyfluoride ceramics by hot pressing and their mechanical, thermal, and electrical properties”, Japanese Journal of Applied Physics 57, 06JF04 (2018) [Non-Patent Document 2] “Fluorine and oxygen plasma exposure behavior of yttrium oxyfluoride ceramics”, Japanese Journal of Applied Physics 58, SEEC01 (2019) [Non-Patent Document 3] "Development of low-dust generating materials with excellent plasma resistance", Ceramics 50 (2015) No.6 490-491 [Non-Patent Document 4] “Examples of Color Tolerances”, [online], Nippon Denshoku Industries Co., Ltd., [Retrieved November 4, 2020], Internet<https: / / www.nippondenshoku.co.jp / web / japanese / colorstory / 08_allowance_by_color.htm> [Non-Patent Document 5] "Effect of rare earth additives on the transparency of α-SiAlON ceramics", Abstracts of the 33rd Autumn Symposium (lecture number 2F27) [Patent documents]
[0005] [Patent Document 1] JP 2016-098143 A [Patent Document 2] International Publication No. 2018 / 159713 Summary of the Invention [Problem to be solved by the invention]
[0006] According to Non-Patent Document 2, Y2 O 3 It has been pointed out that when exposed to fluorine plasma, a layer of alteration due to fluorination is formed on the surface of the yttrium oxide fluoride, e.g., Y 5 O 4 F 7 In the case of YOF, such a degenerated layer does not form, and Y 2 O 3 It is expected to be a next-generation corrosion-resistant material that will replace Y. 5 O 4 F 7 is Y 2 O 3 It has been reported that the change in surface roughness before and after etching with halogen gas is smaller than that of Y and YOF. 5 O 4 F 7 It is believed that the amount of particles generated will be smaller and their size will be smaller than that of Y. 2 O 3 and YOF.
[0007] Hardness is also important for semiconductor manufacturing equipment components. If the hardness is low, the surface is easily scratched during the assembly and maintenance of the equipment. If the resulting scratches are exposed to plasma, they can cause abnormal discharge, become a source of particle generation, and other problems, which is undesirable.
[0008] In addition, Non-Patent Document 3 describes Y 2 O 3 The paper discloses the results of evaluating the plasma resistance of Y by the AD method, which has a larger Vickers hardness. 2 O 3 However, it has been reported that the plasma resistance is higher than that of other manufacturing methods. This result is thought to be due to the fact that a higher hardness increases resistance to the physical action of the etching gas. In other words, even if the chemical composition is the same, the material with a higher hardness has a higher plasma resistance.
[0009] Regarding the Vickers hardness, there is no report in Patent Document 1, and a value of 0.491 [GPa] is reported in Non-Patent Document 1. However, this value is 2 O 3 This is an extremely small value, less than 1 / 12 of the approximately 6.0 GPa of the conventional plasma. Therefore, there are concerns about its plasma resistance, especially its sputter resistance due to ion bombardment.
[0010] High hardness Y 5 O 4 F 7 If it were possible to manufacture such a material, it would be possible to obtain a semiconductor manufacturing equipment component that has high plasma resistance and generates little dust.
[0011] The present invention has been made in consideration of the above problems, and provides a sintered body, a method for manufacturing a sintered body, a semiconductor manufacturing apparatus, and a method for manufacturing a semiconductor manufacturing apparatus that can solve at least any of the various drawbacks described above. [Means for solving the problem]
[0012] The sintered body according to the present invention is Y 5 O 4 F 7 It contains 50% by mass or more, has a relative density of 97.0% or more, and has a Vickers hardness of 2.4 GPa or more.
[0013] In the sintered body, the relative density may be 99.0% or more.
[0014] The sintered body may have an appearance color of white having an L* value of 65 or more in the Lab color space.
[0015] The sintered body may contain 10% by mass or less of at least one of an oxide of a lanthanoid, a fluoride of a lanthanoid, and an oxyfluoride of a lanthanoid.
[0016] The method for producing a sintered body according to the present invention comprises the steps of: 5 O 4 F 7A step of molding a molded body containing the powder, and -3 forming a sintered body by sintering the molded body at a temperature of 1000[°C] or higher in a vacuum atmosphere of Y 5 O 4 F 7 and selecting the sintered body having a relative density of 97.0% or more and a Vickers hardness of 2.4 GPa or more.
[0017] In the method for producing a sintered body, in the step of molding the molded body, the molded body may be molded by a slip casting method or a uniaxial pressing method.
[0018] In the method for producing the sintered body, in the step of forming the sintered body, the sintered body may be formed by a pressureless sintering method at a temperature of 1000° C. or higher and 1400° C. or lower.
[0019] The method for manufacturing the sintered body may further include a step of subjecting the sintered body to a hot isostatic pressing (HIP) process after the step of forming the sintered body, and in the step of selecting the sintered body, the sintered body may be selected from the sintered bodies that have been HIP-treated.
[0020] In the method for producing a sintered body, the relative density of the sintered body before the step of subjecting the sintered body to HIP treatment may be 90% or more.
[0021] In the above-mentioned method for producing a sintered body, the relative density of the sintered body prior to the step of HIP-treating the sintered body may be 94% or more, and the appearance color may be white with an L* value of 75 or more in the Lab color space.
[0022] In the above-mentioned method for manufacturing a sintered body, in the step of molding the molded body, the molded body may be molded by a uniaxial pressing method, and in the step of forming the sintered body, the sintered body may be formed by hot pressing at a temperature of 1000°C or higher and 1400°C or lower.
[0023] In the above-mentioned method for producing a sintered body, in the step of selecting the sintered body, the sintered body having the relative density of 99.0% or more may be selected.
[0024] In the method for producing a sintered body described above, in the step of selecting the sintered body, the sintered body may be selected which has an appearance color of white with an L* value of 65 or more in the Lab color space.
[0025] A semiconductor manufacturing apparatus according to the present invention may include the above-mentioned sintered body.
[0026] The method for manufacturing a semiconductor manufacturing apparatus according to the present invention may further include, after the step of selecting the sintered body in the method for manufacturing a sintered body described above, a step of applying the selected sintered body to a member of the semiconductor manufacturing apparatus. Effect of the Invention
[0027] According to the present invention, it is possible to provide a sintered body capable of improving corrosion resistance, a manufacturing method for a sintered body, a semiconductor manufacturing apparatus, and a manufacturing method for a semiconductor manufacturing apparatus. [Brief description of the drawings]
[0028] [Figure 1] FIG. 2 is a flow chart illustrating a method for producing a sintered body according to the first embodiment. [Diagram 2] FIG. 2 is a flow chart illustrating a method for producing a sintered body according to the first embodiment. [Diagram 3] FIG. 2 is a flow chart illustrating a method for producing a sintered body using the pressureless sintering method according to the first embodiment. [Figure 4] FIG. 2 is a flow chart illustrating a method for producing a sintered body using the pressureless sintering method according to the first embodiment. [Diagram 5] FIG. 2 is a flow chart illustrating a method for producing a sintered body using a hot press method according to the first embodiment. [Figure 6]1 is a graph illustrating the temperature and pressure profiles of hot pressing in the method for producing a sintered body according to the first embodiment, where the horizontal axis indicates time and the vertical axis indicates temperature and pressure. [Figure 7] FIG. 2 is a diagram illustrating evaluation results of a sintered body produced by the pressureless sintering method according to the first embodiment. [Figure 8] FIG. 2 is a diagram illustrating the results of XRD analysis of a sintered body produced by the pressureless sintering method according to the first embodiment. [Figure 9] FIG. 2 is a diagram illustrating the evaluation results of a sintered body produced by a hot press method according to the first embodiment. [Figure 10] FIG. 2 is a diagram illustrating the results of XRD analysis of a sintered body produced by the hot pressing method according to the first embodiment. [Figure 11] FIG. 4 is a diagram illustrating an example of an evaluation result of a sintered body obtained by the pressureless sintering method according to the first embodiment and further subjected to a HIP treatment. [Figure 12] FIG. 2 is a diagram illustrating the results of XRD analysis of a sintered body obtained by the pressureless sintering method according to the first embodiment and further subjected to HIP treatment. [Figure 13] FIG. 4 is a diagram illustrating evaluation results obtained by changing the criteria for the sintered body produced by the pressureless sintering method according to the first embodiment. [Figure 14] FIG. 4 is a diagram illustrating evaluation results obtained by changing the criteria for the sintered body produced by the hot press method according to the first embodiment. [Figure 15] FIG. 2 is a diagram illustrating the production conditions and plasma resistance test results of the sintered body according to the first embodiment. [Figure 16] FIG. 11 is a configuration diagram illustrating a semiconductor manufacturing apparatus according to a second embodiment. [Figure 17] FIG. 11 is a flow chart illustrating a manufacturing method of a semiconductor manufacturing apparatus according to a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] For clarity of explanation, the following description and drawings are omitted and simplified as appropriate. In addition, in each drawing, the same elements are given the same reference numerals, and duplicate explanations are omitted as necessary.
[0030] (Embodiment 1) The sintered body and the manufacturing method of the sintered body according to the first embodiment will be described below. First, the outline of the sintered body will be described. Then, the manufacturing method of the sintered body will be described. After that, the evaluation method of the sintered body and the evaluation results will be described.
[0031] <Overview of sintered body> The inventors have conducted extensive research and have developed a high-density, high-hardness Y 5 O 4 F 7 Specifically, the obtained sintered body was Y 5 O 4 F 7 The sintered body of this embodiment contains 50% by mass or more of Y, has a relative density of 97.0% or more, and has a Vickers hardness of 2.4 GPa or more. As described above, the sintered body of this embodiment has a high relative density, and therefore can improve corrosion resistance. 5 O 4 F 7 The sintered body has a relative density of 99.0% or more. This improves corrosion resistance against halogen gas. 5 O 4 F 7 The sintered body is Y 2 O 3 The sintered body of this embodiment is expected to be a next-generation corrosion-resistant material that will replace Y. 2 O 3 In this way, the sintered body of the present embodiment has high hardness, and therefore can improve plasma resistance. 5 O 4 F 7 The sintered body contains Y as the main phase. 5 O 4 F 7 It is possible to make the content 99% by mass or more, thereby improving the quality.
[0032] On the other hand, Y 5 O 4 F 7It has been found that when attempting to sinter at high temperatures to increase density, the resulting sintered body may turn black. The discoloration is thought to be caused by the loss of oxygen (O) and fluorine (F) due to high temperatures, or the diffusion and aggregation of carbon. If the components inside the chamber of a semiconductor manufacturing device are black, it becomes difficult to visually check for black stains caused by abnormal discharges in the chamber, and abnormalities may be overlooked. In addition, problems such as preventing the determination of opportunities for chamber cleaning occur. Therefore, it is preferable for the components inside the chamber to be white, so that stains are easily visible.
[0033] As a result of careful consideration of the manufacturing conditions, the inventors have found that such a high density, high hardness Y 5 O 4 F 7 We succeeded in forming a sintered body of Y without discoloring it black. 5 O 4 F 7 The sintered body has an appearance color of white with an L* value of 65 or more in the Lab color space. Since the appearance color is almost white, stains due to abnormal discharges or the like in semiconductor manufacturing equipment can be easily confirmed by visual inspection or image recognition. Therefore, detection of abnormal discharges and cleaning of components can be easily performed.
[0034] Y 5 O 4 F 7 The sintered body may contain at least one of lanthanoid oxide, lanthanoid fluoride, and lanthanoid oxyfluoride in an amount of 10% by mass or less. By adding a small amount of a so-called "auxiliary agent" before sintering, the sinterability can be improved. In addition, the microstructure of the sintered body can be controlled.
[0035] <Method of manufacturing sintered body> Next, the manufacturing method of the sintered body of the present embodiment will be described. FIGS. 1 and 2 are flowchart diagrams illustrating the manufacturing method of the sintered body according to Embodiment 1. As shown in FIG. 1, the manufacturing method of the sintered body according to the present embodiment includes a step SA of molding a molded body, a step SB of forming a sintered body, and a step SS of selecting a sintered body. In step SA of molding a molded body, a molded body containing 5 O 4 F 7 powder is molded. In step SB of forming a sintered body, a sintered body is formed by sintering the molded body. In step SS of selecting a sintered body, a desired sintered body is selected from the obtained sintered bodies. For example, as an example, in step SS of selecting a sintered body, 5 O 4 F 7 A sintered body containing 50 [mass%] or more, having a relative density of 97.0 [%] or more, and a Vickers hardness of 2.4 [GPa] or more is selected.
[0036] Note that, as shown in FIG. 2, the manufacturing method of the sintered body may include a step SC of subjecting the sintered body to hot isostatic pressing (hereinafter referred to as HIP) treatment between step SB of forming the sintered body and step SS of selecting the sintered body.
[0037] In the manufacturing method of the sintered body of the present embodiment, step SB of forming the sintered body can be divided into a method using a non-pressure sintering method and a method using a hot pressing method. Therefore, hereinafter, it will be described separately as I. A manufacturing method of a sintered body using a non-pressure sintering method and II. A manufacturing method of a sintered body using a hot pressing method.
[0038] <I. A manufacturing method of a sintered body using a non-pressure sintering method> 3 and 4 are flow charts illustrating a method for manufacturing a sintered body using the pressureless sintering method according to the first embodiment. As shown in FIG. 3, the method for manufacturing a sintered body using the pressureless sintering method includes a step S11 of preparing raw material powder and a molding step S12 as a step SA for molding a molded body. A debinding step S13 may be performed after the molding step S12. A pressureless sintering step S14 is included as a step SB for forming a sintered body. A step SS for selecting a sintered body includes a step S15. Note that, as shown in FIG. 4, a cold isostatic pressing (hereinafter referred to as CIP) processing step S12a may be added as a molding step SA after the molding step S12. After that, a debinding step S13 or a pressureless sintering step S14 may be performed.
[0039] Below, I. A method for manufacturing a sintered body using pressureless sintering will be explained in the following order: 1. Preparation of raw material powder (step S11), 2. Molding (step S12), 3. CIP treatment (step S12a), 4. Degreasing (step S13), and 5. Pressureless sintering (step S14).
[0040] <1. Preparation of raw powder> The raw material powder is Y 5 O 4 F 7 The raw powder is Y 5 O 4 F 7 Three types of powder are used: a powder with a particle size of 0.5 μm (hereinafter referred to as raw material powder A), a powder with a particle size of 0.8 μm (hereinafter referred to as raw material powder B), and a powder with a particle size of 1.0 μm (hereinafter referred to as raw material powder C).
[0041] <2. Molding> Next, as molding methods for the molded body, 2-1. Slip cast method and 2-2. Press method (uniaxial pressure method) will be explained. In the manufacturing method for the sintered body using the pressureless sintering method, in the molding step, the molded body is molded by the slip cast method or the uniaxial pressure method.
[0042] <2-1. Slip casting method> The slip casting method is also called the casting method. The slip casting method includes a slurry preparation process and a slip casting molding process.
[0043] In the slurry preparation process, for example, 100 g of raw material powder A, 50 g of ethanol as a solvent, 2 g of dispersant, and 10 mL of a solution in which 2.3 g of binder is dissolved in 50 mL of ethanol are mixed in a glass container to prepare a slurry for slip casting. Slurries for slip casting are also prepared for raw material powders B and C in the same manner.
[0044] In the slip cast molding process, the prepared slurry is poured into a silicone mold (diameter 13.5 mm, depth 20 mm) placed on a plaster board. It is then left to stand for four days. Once it has been confirmed that the ethanol has been absorbed into the plaster board or evaporated and that it is sufficiently dry, it is removed from the silicone mold. This results in a molded body (diameter approximately 13.5 mm, height approximately 7 mm).
[0045] <2-2. Press method> The pressing method includes a step of preparing powder for pressing and a step of press molding.
[0046] In the preparation process of the powder for pressing, for example, 100 g of raw material powder A, 25 g of pure water as a solvent, 0.3 g of dispersant, and 4.4 mL of a solution in which the binder is dissolved in 12 mL of pure water are mixed in a glass container to prepare a binder-added slurry that is the source of the powder for pressing. The prepared slurry is then freeze-dried to remove the pure water and obtain the powder for pressing. The raw material powders B and C are also prepared in the same manner to obtain the powder for pressing.
[0047] In the press molding process, 2.0 g of the obtained powder for pressing is placed in a cylindrical mold with a diameter of 10 mm, and a pressure of 8 MPa is applied using a hydraulic press. After that, it is removed from the mold to obtain a molded body with a diameter of about 10 mm and a height of about 8 mm.
[0048] <3. CIP processing> The molded bodies obtained by the above 2-1. Slip casting method and 2-2. Pressing method may be subjected to CIP treatment to further densify them before sintering. Specifically, the molded bodies are vacuum packed, and then pressurized at a pressure of 300 MPa for 10 min using a CIP device.
[0049] <4. Degreasing> In order to remove the binder component and dispersant component contained in the molded body, the molded body obtained by the above 2-1. slip casting method and 2-2. pressing method, and the molded body further subjected to CIP treatment are heated under various conditions and degreased. When heating, for example, the molded body is placed on an alumina plate and heated. Specifically, the molded body is heated at a temperature of 400[°C] in a nitrogen gas atmosphere (for example, flow rate of 0.2 L / min). The molded body molded by 2-1. slip casting method is heated for, for example, 100[h], and the molded body molded by 2-2. pressing method is heated for, for example, 50[h].
[0050] <5. Pressureless sintering method> The degreased molded body is placed in, for example, an alumina crucible, covered with a lid, and sintered in an electric furnace under various conditions. The sintering conditions are as follows: argon (Ar) gas (flow rate 2 [L / min]), nitrogen (N 2 ) in gas (flow rate 2 [L / min]) or vacuum (approx. 10 -3 The heating rate is set to 1000[℃ / h], the holding temperature is set to 900 to 1400[℃], the holding time is set to 0 to 3[h], and the cooling rate is set to furnace cooling.
[0051] The reason for setting the maximum holding temperature at 1400°C was that in a previous experiment, the Y 5 O4 F 7 When the sintered sample was subjected to XRD analysis, peaks derived from YOF other than Y 5 O 4 F 7 powder were detected. When sintering was carried out at 1400 [°C], no peak derived from YOF was observed. Therefore, when sintering at a high temperature exceeding 1400 [°C], it is considered that F of Y 5 O 4 F 7 desorbs and the YOF phase appears. As described above, since Y 5 O 4 F 7 has higher plasma resistance than YOF, it is not preferable that YOF is mixed into Y 5 O 4 F 7 . Therefore, the maximum holding temperature is set to 1400 [°C].
[0052] As shown in FIG. 2, in the method for manufacturing a sintered body using the uniaxial sintering method, after step 5. Uniaxial sintering (step S14) of step SB for forming the sintered body, HIP treatment may be further performed. Thereby, the sintered sintered body can be further densified.
[0053] <6. HIP treatment> Put the sintered body into an alumina crucible, cover it, and using a HIP apparatus, set the pressure under an argon atmosphere to 200 [MPa], the heating rate to 1000 [°C / h], the holding temperature to 900 to 1100 [°C], and the holding time to 0 to 3 [h].
[0054] <II. Method for manufacturing a sintered body using the hot press method> Next, a method for producing a sintered body using the hot press method will be described. FIG. 5 is a flow chart illustrating a method for producing a sintered body using the hot press method according to the first embodiment. As shown in FIG. 5, the method for producing a sintered body using the hot press method includes step S31 of preparing raw material powder and molding step S32 as step SA for molding a molded body. Step SB for forming a sintered body includes step S33 of hot pressing. Step SS for selecting a sintered body includes step S34. Below, the method for producing a sintered body using the hot press method will be described in the order of 1. Preparation of raw material powder (step S31), 2. Primary molding method (step S32), and 3. Hot pressing (step S33). Note that, in the method for producing a sintered body using the hot press method, as shown in FIG. 2, HIP treatment may be further performed after hot pressing (step S33) in step SB.
[0055] <1. Raw material powder> The raw powder is processed in the same manner as in I. Manufacturing method of sintered body using pressureless sintering method. 5 O 4 F 7 The raw powder is Y 5 O 4 F 7 Three types of powder are used: a powder with a particle size of 0.5 μm (hereinafter referred to as raw material powder A), a powder with a particle size of 0.8 μm (hereinafter referred to as raw material powder B), and a powder with a particle size of 1.0 μm (hereinafter referred to as raw material powder C).
[0056] <2.Primary molding method> In the primary molding method using hot press, 100 g of raw material powder A is placed directly into a square mold 50 mm long and 50 mm wide. Then, a pressure of, for example, 18.4 MPa is applied using a hydraulic press. In this way, in the step of molding a molded body, the molded body is molded using a uniaxial pressing method. After that, it is removed from the mold to obtain a primary molded body that is approximately 50 mm long, 50 mm wide, and 12 mm high. A primary molded body can be obtained in the same manner for raw material powder C.
[0057] <3. Hot pressing> The green compact is placed in a hot press mold made of carbon with the same size in the vertical and horizontal directions, and hot pressing is performed under various conditions. Under the conditions of hot pressing, the atmosphere is in argon gas (flow rate 1 [L / min]) or in vacuum (about 10 -3 [Pa] or less).
[0058] Figure 6 is a graph illustrating the profiles of the temperature and pressure of hot pressing in the method for manufacturing a sintered body according to Embodiment 1. The horizontal axis represents time, and the vertical axis represents temperature and pressure. As shown in Figure 6, the heating rate is 10 [°C / min], the holding temperature is 900 to 1400 [°C], the holding time is 0 to 1 [h], and the cooling rate is 10 [°C / min]. Pressure increase starts simultaneously with the start of heating, and the holding pressure is reached in 1 hour. The holding pressure is 36.7 [MPa], the pressure reduction becomes 0 [MPa] in 1 hour, and each is set so that the end of pressure reduction and the end of cooling are simultaneous. Note that for the same reason as described in 5. Non-pressure sintering method in <Method for manufacturing a sintered body using a non-pressure sintering method>, the maximum temperature of the holding temperature is set to 1400 [°C].
[0059] <Method for evaluating the sintered body> Next, a method for evaluating the manufactured sintered body will be described. First, as evaluation methods, 1. density, 2. hardness (Vickers hardness), 3. whiteness, 4. composition analysis, and 5. plasma resistance will be described.
[0060] <1. Density> Using an electronic balance, the weight of the obtained sintered body in the air and the weight in pure water are weighed, and the density is determined by the Archimedes method. The obtained density is divided by the theoretical density 5.14 [g / cm 5 O 4 F 7 of Y 3 to calculate the relative density [%].
[0061] In addition, if there are voids in the material used for semiconductor manufacturing equipment components, those voids will cause concentrated corrosion and become a source of dust. Therefore, materials used for semiconductor manufacturing equipment components are required to have a high density, preferably with a relative density of 97.0% or more, and more preferably with a relative density of 99.0% or more.
[0062] <2. Vickers hardness> Using a hardness tester, measure the Vickers hardness, for example, with a test force of 0.5 gf.
[0063] <3. Whiteness> To quantitatively evaluate whiteness, L*, one of the chromaticities in the Lab color space, is used as an index. In addition, to minimize changes in chromaticity due to surface roughness and other factors on the surface of the sintered body, L* is measured using the SCI (Specular Component Include) method. Specifically, a colorimeter is used to measure L* on the surface of the sintered body.
[0064] In addition, the Y 5 O 4 F 7 It has been confirmed that the a* and b* values in the Lab color space of the sintered body are within the ranges of approximately ±1 and ±5, respectively, and the external color is nearly achromatic (white to black).
[0065] In the semiconductor manufacturing equipment member of Patent Document 2, L* is used as an index for quantitatively evaluating whiteness (blackness). Patent Document 2 also states that "if the color of the member is black, dirt is not noticeable and excessive cleaning is not required, which is preferable." However, if the end point of cleaning is controlled by limit samples or reflectance measurements during cleaning, such a problem does not occur. On the contrary, if dirt is difficult to see, such quantitative control becomes difficult, and as a result, cleaning becomes insufficient, and there is a concern that foreign matter (particles) due to dirt may be generated. In other words, it is preferable that the external color of the semiconductor manufacturing equipment member is white, metallic, or transparent, since dirt can be easily seen.
[0066] Regarding the external color of the component, for example, when an operator of the device performed a sensory evaluation on visual confirmation of stains, it was found that stains were easily visible when L* was 60 to 70 or more. Therefore, it is considered that stains are easily visible when L* is 65 or more.
[0067] Furthermore, as shown in Table 1 of Patent Document 2, the chromaticity L* after exposure to plasma is about 60, so it can be said that the chromaticity L* of the stain caused by exposure to plasma is about L* = 60. In the Lab color space, the color difference between two colors is defined as follows:
[0068] Color difference ΔE=(ΔL* 2 +Δa* 2 +Δb* 2 ) 1 / 2
[0069] Y 5 O 4 F 7 As mentioned above, the sintered body is almost achromatic, and the absolute values of a* and b* are small and their changes are also small, so the color difference ΔE is dominated by the change in L*. Therefore, it is acceptable to replace it with the following formula.
[0070] Color difference ΔE≒ΔL*
[0071] For example, Non-Patent Document 4 states that a color difference ΔE of 5.0 means that "when compared over time, it is recognized as being almost the same," so conversely, if the color difference ΔE is 5.0 or more, it can be said that "when compared over time, a change in color is recognized." In other words, compared to the chromaticity L* of dirt = 60, a member with a color difference ΔE (≒ ΔL*) of 5 or more, in other words, L* of 65 or more, can be said to have dirt that can be visually confirmed.
[0072] <4. Composition analysis> Manufactured by Y 5 O 4 F 7 The sintered body is analyzed using an X-ray diffraction device (XRD) to confirm the composition.
[0073] <5. Plasma resistance test> First, the surface condition of the sample is smoothed. This makes the variation in the surface condition between samples uniform. To smoothen the surface, the surface of the sintered body is polished with waterproof paper of #1000 to #4000. Smoothing is continued until the arithmetic surface roughness (Ra) is approximately 0.1 μm or less.
[0074] Next, in order to secure an area that is not exposed to the plasma treatment, 5 O 4 F 7 Approximately half of the surface of the sintered body is covered with polyimide tape. The sintered body with the polyimide tape attached is placed in an etching device and CF 4 / O 2 A plasma resistance test using mixed gas is carried out. Specifically, the electrode size is 100 mm in diameter, the pressure is 20 Pa, the RF power is 150 W, and the CF 4 The gas flow rate was set to 40 mL / min, and O 2 The gas flow rate is set to 10 mL / min, and plasma treatment is performed for 2 h. After plasma treatment, the sintered body is removed and the polyimide tape is peeled off.
[0075] The boundary portion near the end of the polyimide tape is measured for step height using a surface profiler, and the step height is regarded as the amount of etching. In addition, the surface profiler is used to measure the arithmetic surface roughness (Ra) of the sintered body surface before and after the plasma resistance test for the portion not covered with the polyimide tape. The deterioration rate of the arithmetic surface roughness Ra is calculated using the following formula.
[0076] (Ra deterioration rate)=(Ra after plasma resistance test) / (Ra before plasma resistance test)
[0077] It can be said that the smaller the rate of deterioration of Ra, the less damage to the surface caused by plasma exposure.
[0078] <Evaluation Results> Next, the evaluation results will be explained. The evaluation results will be explained separately for the sintered body by the pressureless sintering method, the sintered body by the hot pressing method, and the sintered body by the pressureless sintering method and the HIP treatment. First, the evaluation results of the sintered body by the pressureless sintering method will be explained.
[0079] <Evaluation results of sintered bodies produced by pressureless sintering method> FIG. 7 is a diagram illustrating the evaluation results of the sintered body by the pressureless sintering method according to the first embodiment. In FIG. 7, the conditions of step SA for molding the molded body and step SB for forming the sintered body are shown as the manufacturing method. For example, in Example 1 in FIG. 7, the conditions of step SA for molding the molded body are that A is used as the raw material powder, and the molded body is molded by the slip casting method. Then, the molded body is subjected to CIP treatment. The conditions of step SB for forming the sintered body are that the sintered body is formed in an argon atmosphere by increasing the temperature at a rate of 1000[°C / h], holding the temperature at 1000[°C], and holding time of 1[h]. The evaluation results are a relative density of 97.2[%], a hardness of 3.9[GPa], and a whiteness L* of 81.31. The overall evaluation is ⊚.
[0080] Here, an overall rating of ⊚ indicates that the density is 97.0% or more, the hardness is 2.4 GPa or more, and the whiteness L* is 65 or more. An overall rating of ◯ indicates that the density is 97.0% or more, the hardness is 2.4 GPa or more, and the whiteness L* is less than 65. An overall rating of × indicates that the density is less than 97.0% or the hardness is less than 2.4 GPa.
[0081] As shown in Figure 7, the 10 -3 By sintering the molded body at a temperature of 1000°C or higher in a vacuum atmosphere of 0.01 Pa or less, a Y-type sintered body having a relative density of 97.0% or more and a Vickers hardness of 2.4 GPa or more is obtained. 5 O 4 F 7 For example, in the step SB for forming the sintered body, the above Y can be obtained by a pressureless sintering method at a temperature of 1000° C. or more and 1400° C. or less. 5 O 4F 7 It is possible to form a sintered body. In addition, as the relative density increases, the whiteness L* tends to increase.
[0082] Fig. 8 is a diagram illustrating the results of XRD analysis of the sintered body obtained by the pressureless sintering method according to embodiment 1. In addition to Examples 1 and 2 and Comparative Example 16, Fig. 8 also shows the results of XRD analysis of raw material powder A. As shown in Fig. 8, raw material powder A contains almost no impurities. The results of XRD analysis of raw material powders B and C are also similar to that of raw material powder A.
[0083] In addition, Y produced using raw material powder A 5 O 4 F 7 The sintered body also showed almost no impurity peaks, and the Y 5 O 4 F 7 The sintered body is essentially Y 5 O 4 F 7 That is, Y 5 O 4 F 7 The sintered body is Y 5 O 4 F 7 The same XRD analysis results were compared with those of other examples. 5 O 4 F 7 It can also be obtained from a sintered body.
[0084] From the above, according to this embodiment, it is possible to obtain Y having a relative density of 97.0% or more and a Vickers hardness of 2.4 GPa or more. 5 O 4 F 7 A sintered body can be formed. 5 O 4 F 7 Y contains 99% by mass or more, has a relative density of 97.0 to 99.3%, and has a Vickers hardness of 2.4 to 4.4 GPa. 5 O 4 F 7 A sintered body can be formed.
[0085] Such a Y 5 O 4 F 7 The sintered body has both high density and high hardness, and can improve plasma resistance. 5 O 4 F 7 The sintered body can be manufactured by a pressureless sintering method, which has a high degree of freedom in shape. In particular, when a slip casting method, which is a mold molding method, is used for molding, the degree of freedom in shape is very high, and the production cost can be reduced by the so-called near net shape. 5 O 4 F 7 It was not possible to obtain a sintered sample having a relative density of 99.0% or more and a whiteness L* of 65 or more within the range of manufacturing conditions shown in FIG.
[0086] <Evaluation results of sintered bodies using hot pressing method> FIG. 9 is a diagram illustrating the evaluation results of the sintered body by the hot pressing method according to the first embodiment. In FIG. 9, the manufacturing conditions are shown as the conditions of step SA for molding the molded body and step SB for forming the sintered body. For example, in Example 14 in FIG. 9, A is used as the raw material powder, and the sintered body is formed in an argon atmosphere at a holding temperature of 1000[°C] and a holding time of 1[h]. The evaluation results are a relative density of 100[%], a Vickers hardness of 2.4[GPa], and a whiteness L* of 40.32. The overall evaluation is ◯. The meanings of ◎, ◯, and × are the same as those described above.
[0087] As shown in Fig. 9, when the holding temperature is 900°C or higher and the holding time is 1 h, or when the holding temperature is 1000°C or higher and there is no holding time, the relative density is 97% or higher and the Vickers hardness is 2.4 GPa or higher. 5 O 4 F 7 For example, in the step SB for forming the sintered body, the above Y can be obtained by hot pressing at a temperature of 900° C. or more and 1400° C. or less.5 O 4 F 7 A sintered body can be formed.
[0088] Fig. 10 is a diagram illustrating the results of XRD analysis of the sintered body produced by the hot pressing method according to embodiment 1. In addition to Examples 7 and 9 and Comparative Example 28, Fig. 10 also shows the results of XRD analysis of raw material powder A. As shown in Fig. 10, raw material powder A contains almost no impurities. The results of XRD analysis of raw material powders B and C are also similar to that of raw material powder A.
[0089] In addition, almost no impurity peaks were observed in any of the sintered bodies, and the sintered bodies according to the present embodiment were substantially Y 5 O 4 F 7 It can be confirmed that the sintered body consists only of ZnO. Similar XRD analysis results can also be obtained from the sintered bodies of the other Examples. However, it was not possible to obtain a sample with a relative density of 97.0% or more and a whiteness L* of 65 or more within the range of manufacturing conditions shown in Figure 9.
[0090] <Evaluation results of sintered bodies produced by pressureless sintering and HIP treatment> Fig. 11 is a diagram illustrating the evaluation results of a sintered body obtained by further HIP-treating the sintered body by the pressureless sintering method according to the first embodiment. Fig. 11 shows the manufacturing conditions and evaluation results of the sintered body before HIP-treating, the HIP-treating conditions, and the evaluation results after HIP-treating. For example, in Example 25 in Fig. 11, the sintered body of Example 1 is used as the sintered body before HIP-treating. The overall evaluation at this point is J◎.
[0091] Here, an overall judgement of J◎ for the sintered body before HIP treatment indicates that the density is 94.0[%] or more and the whiteness L* is 75 or more. An overall judgement of J● indicates that the density is 94.0[%] or more and the whiteness L* is less than 75. An overall judgement of J〇 indicates that the density is 90.0[%] or more and less than 94.0[%]. An overall judgement of J× indicates that the density is less than 90.0[%].
[0092] For example, in Example 25, the HIP treatment was performed at a holding temperature of 1100°C and for a holding time of 3 hours. The evaluation results were a relative density of 99.5%, a Vickers hardness of 2.9 GPa, and a whiteness L* of 67.27. The overall evaluation was ◎. The meanings of the overall evaluations ◎, ◯, and × are the same as those in <Evaluation results of sintered bodies by pressureless sintering method> and <Evaluation results of sintered bodies by hot pressing method>.
[0093] As shown in Fig. 11, when a sintered body with a relative density of 90% or more is HIP-treated at 1000°C or higher for 0 to 3 hours, a Y with a relative density of 97% or more and a Vickers hardness of 2.4 GPa or more is obtained. 5 O 4 F 7 Furthermore, when a sintered body having a density of 94.0% or more and an L* of 75 or more is subjected to HIP treatment under the above conditions, a Y compact having a relative density of 97.0% or more, a Vickers hardness of 2.4 GPa or more, and an L* of 65 or more can be obtained. 5 O 4 F 7 A sintered body can be obtained.
[0094] In this way, Y in this embodiment 5 O 4 F 7 Sintered bodies can also be obtained by subjecting pressureless sintered bodies to HIP treatment, in which they are isotropically pressed, which allows for greater freedom in shape than the hot press method, in which pressure is applied uniaxially and sintered.
[0095] Fig. 12 is a diagram illustrating the results of XRD analysis of a sintered body obtained by further HIP-treating the sintered body produced by the pressureless sintering method according to embodiment 1. Fig. 12 also shows the results of XRD analysis of raw material powder C in addition to Examples 22 and 25. As shown in Fig. 12, raw material powder C contains almost no impurities.
[0096] In addition, almost no impurity peaks were observed in any of the sintered bodies, and the sintered bodies according to the present embodiment were substantially Y 5 O 4 F 7It can be confirmed that the sintered body consists of only .Also, similar XRD analysis results can be obtained from the sintered bodies according to the other examples.
[0097] The sintered body before HIP treatment preferably has a relative density of 90% or more. Alternatively, the sintered body before HIP treatment preferably has a relative density of 94.0% or more and a whiteness L* of 75 or more. Therefore, the preferable conditions for such a sintered body before HIP treatment are considered below.
[0098] Fig. 13 is a diagram illustrating the evaluation results when the judgment criteria are changed for the sintered body by the pressureless sintering method according to the embodiment 1. As shown in Fig. 13, if the holding temperature is 900[°C] or more and the holding time is 1[h], a sintered body having a relative density of 90[%] or more can be obtained. Also, if the holding temperature is 1000[°C] or more and the holding time is 1[h], a sintered body having a relative density of 94.0[%] or more and a whiteness L* of 75 or more can be obtained.
[0099] Fig. 14 is a diagram illustrating the evaluation results when the judgment criteria are changed for the sintered body by the hot pressing method according to the embodiment 1. As shown in Fig. 14, a sintered body having a relative density of 90% or more can be obtained at a holding temperature of 900 to 1400°C for a holding time of 0 to 1 h. Also, in an argon atmosphere, a sintered body having a relative density of 94.0% or more and a whiteness L* of 75 or more can be obtained at a holding temperature of 1000°C for a holding time of 0 h.
[0100] FIG. 15 is a diagram illustrating the manufacturing conditions and plasma resistance test results of the sintered body according to the embodiment 1. For comparison, FIG. 2 O 3 The results of the plasma resistance test for the sintered body are also shown in the same manner (Comparative Example 36). As shown in FIG. 15, the sintered bodies of Examples 1, 23, and 34 have a plasma resistance of 0.1%. 2 O 3 Compared to the sintered body, the etching amount is equal to or less than that of the sintered body, and the change in surface roughness is also small. 5 O 4 F 7The sintered body is Y 2 O 3 Compared to sintered bodies, it has high plasma resistance overall, and is particularly advantageous in terms of reducing the amount of dust generated, which is the most important point.
[0101] The sintered body of Example 23 has a small whiteness L*, which is thought to make stains less visible, but the plasma resistance is comparable to that of a sintered body with a large whiteness L*. In other words, the whiteness L* value affects the visibility of stains, but has almost no effect on the plasma resistance, which is important for semiconductor manufacturing equipment members.
[0102] Comparing Example 1 and Comparative Example 18, the etching amount and the rate of deterioration of Ra are smaller in Example 1, and the plasma resistance is better. The hardness of both is almost the same, but there is a difference in the relative density. Considering that the whiteness L* value has almost no effect on the plasma resistance, it can be said that the poor plasma resistance of Comparative Example 18 is due to the low relative density. In other words, if the relative density is less than 97[%], corrosion progresses from the voids, and the plasma resistance deteriorates. Therefore, the relative density is preferably 97[%] or more.
[0103] Moreover, comparing Example 23 and Comparative Example 27, the etching amount and the Ra deterioration rate are smaller in Example 23, and the plasma resistance is better. The relative density of both is almost the same, but there is a difference in hardness. Considering that the whiteness L* value has almost no effect on the plasma resistance, it can be said that the poor plasma resistance of Comparative Example 27 is due to the low hardness. If the hardness is less than 2.4 [GPa], physical etching proceeds and the plasma resistance deteriorates. Therefore, the hardness is preferably 2.4 [GPa] or more.
[0104] <About auxiliary agents> Next, the auxiliary agent will be described. In general, in the manufacture of ceramics, in addition to the base material, a small amount of additives, so-called "auxiliary agents," is added in the range of several to 10% by mass before sintering. This enhances the sinterability and controls the microstructure of the sintered body. For example, Non-Patent Document 5 discloses a method of adding rare earth elements to control the microstructure of SiAlON ceramics and reduce the grain size to improve the optical properties.
[0105] The sintered body of this embodiment can also be produced by sintering using an auxiliary agent. 5 O 4 F 7 It is defined as "consisting of". By using an auxiliary to control the microstructure, it is possible to further improve the plasma resistance. For example, the auxiliary can be unevenly distributed in the grain boundary region where plasma resistance is low, thereby improving the plasma resistance of the grain boundary region. In addition, dust generation can be reduced by controlling the particle size. By increasing the particle size, the proportion of the grain boundary region where plasma resistance is low can be reduced, and the etching rate can be reduced. Conversely, by decreasing the particle size, the size of the particles generated can be reduced.
[0106] In the sintered body of this embodiment, the material used as the auxiliary is Y 5 O 4 F 7 Similarly, it is desirable that the plasma resistance is high. In general, rare earth elements, particularly lanthanoid elements (La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu), have a relatively low vapor pressure when combined with halogens compared to other elements, and have excellent plasma resistance. Oxides, fluorides, and oxyfluorides, which are stable compounds of these elements, are preferred as auxiliary agents to be added in the present invention.
[0107] (Embodiment 2) Next, a semiconductor manufacturing apparatus and a method for manufacturing the semiconductor manufacturing apparatus according to the second embodiment will be described. The semiconductor manufacturing apparatus of this embodiment is provided with the sintered body of the first embodiment. FIG. 16 is a configuration diagram illustrating the semiconductor manufacturing apparatus according to the second embodiment. As shown in FIG. 16, the semiconductor manufacturing apparatus 1 of this embodiment has, for example, a chamber 10. The semiconductor manufacturing apparatus 1 is, for example, an etching apparatus, but is not limited thereto and may be other semiconductor manufacturing apparatus such as a chemical vapor deposition apparatus. The inner wall of the chamber 10 or a member used within the chamber includes a sintered body 20. The sintered body 20 may be, for example, the Y-type sintered body described in the first embodiment. 5 O 4 F 7 It is a sintered body.
[0108] FIG. 17 is a flow chart illustrating a method for manufacturing a semiconductor manufacturing apparatus according to the second embodiment. As shown in FIG. 17, the method for manufacturing a semiconductor manufacturing apparatus includes a step of manufacturing a sintered body (step S100) and a step of applying the sintered body to a member of the semiconductor manufacturing apparatus (step S200). Here, the step S100 for manufacturing a sintered body includes a step SA for molding the molded body in FIG. 1 or FIG. 2 of the first embodiment, a step SB for forming a sintered body, a step SC for HIP-treating the sintered body, and a step SS for selecting a sintered body. The step SS for selecting a sintered body selects a desired sintered body from the obtained sintered bodies. For example, Y 5 O 4 F 7 A sintered body containing 50% by mass or more, having a relative density of 97.0% or more, and having a Vickers hardness of 2.4 GPa or more is selected. In step SS of selecting a sintered body, a sintered body having a relative density of 99.0% or more may be selected, or a sintered body having an appearance color of white with an L* value of 65 or more in the Lab color space may be selected. Furthermore, a sintered body may be selected from sintered bodies that have been subjected to HIP processing.
[0109] In step S200 of applying the sintered body to members of the semiconductor manufacturing equipment, after step SS of selecting a sintered body in the manufacturing method of the sintered body, the selected sintered body is applied to members of the semiconductor manufacturing equipment 1. For example, the sintered body is applied to members of the inner walls of the chamber 10 or the like or members of parts used in the chamber.
[0110] In the semiconductor manufacturing apparatus 1 of this embodiment, the inner wall of the chamber 10, etc. is 5 O 4 F 7 Providing a sintered body can improve the corrosion resistance, for example, the plasma resistance, of the semiconductor manufacturing equipment 1. Other configurations and effects are included in the description of the first embodiment.
[0111] The present invention is not limited to the above-described embodiment, and may be modified as appropriate without departing from the spirit and scope of the present invention. For example, the configurations of the embodiment and the modifications may be combined with each other. [Explanation of symbols]
[0112] 1. Semiconductor manufacturing equipment 10. Chamber 20 Sintered body
Claims
1. Y 5 O 4 F 7 The sintered body has a relative density of 97.0% or more and a Vickers hardness of 2.4 GPa or more.
2. The relative density is 99.0% or more. The sintered body according to claim 1 .
3. The appearance color is white with an L* of 65 or more in the Lab color space; The sintered body according to claim 1 or 2.
4. Contains at least one of an oxide of a lanthanoid, a fluoride of a lanthanoid, and an oxyfluoride of a lanthanoid in an amount of 10 [mass%] or less. The sintered body according to any one of claims 1 to 3.
5. Y 5 O 4 F 7 Molding a molded body containing the powder; Argon gas atmosphere or 10 -3 sintering the molded body at a temperature of 1000° C. or higher in a vacuum atmosphere of 0.1 Pa or lower to form a sintered body; Y 5 O 4 F 7 selecting the sintered body having a relative density of 97.0% or more and a Vickers hardness of 2.4 GPa or more; A method for producing a sintered body comprising the steps of:
6. In the step of molding the molded body, The molded body is molded by a slip casting method or a uniaxial pressing method. A method for producing the sintered body according to claim 5.
7. In the step of forming the sintered body, The sintered body is formed by a pressureless sintering method at a temperature of 1000° C. or more and 1400° C. or less. A method for producing the sintered body according to claim 5 or 6.
8. The method further includes the step of subjecting the sintered body to a HIP treatment after the step of forming the sintered body. In the step of selecting the sintered body, the sintered body is selected from the sintered bodies that have been subjected to HIP treatment. A method for producing the sintered body according to claim 7.
9. The relative density of the sintered body before the step of subjecting the sintered body to HIP treatment is 90% or more. A method for producing the sintered body according to claim 8.
10. In the sintered body before the step of subjecting the sintered body to HIP treatment, the relative density is 94% or more, and the L* in the Lab color space of the appearance color is white of 75 or more. A method for producing the sintered body according to claim 8.
11. In the step of molding the molded body, The molded body is molded by a uniaxial pressing method, In the step of forming the sintered body, The sintered body is formed by hot pressing at a temperature of 1000° C. or more and 1400° C. or less. A method for producing the sintered body according to claim 5.
12. In the step of selecting the sintered body, the sintered body having the relative density of 99.0% or more is selected. The method for producing the sintered body according to any one of claims 5 to 11.
13. In the step of selecting the sintered body, the sintered body is selected which has an appearance color of white with an L* value of 65 or more in the Lab color space. The method for producing the sintered body according to any one of claims 5 to 12.
14. A semiconductor manufacturing device comprising the sintered body according to any one of claims 1 to 4.
15. A method for manufacturing a semiconductor manufacturing apparatus, further comprising a step of applying the selected sintered body to a member of a semiconductor manufacturing apparatus after the step of selecting the sintered body in the method for manufacturing a sintered body according to any one of claims 5 to 13.
Citation Information
Patent Citations
Sintered body
JP2016098143A
Sintered body
JP2016153369A
Method for manufacturing fluoride ceramics sintered body
JP2019069876A
Method for forming yttrium fluoride oxide coating film and yttrium fluoride oxide coating film obtained by the method
JP2020525640A
Rare earth oxyfluoride sintered body and method for producing same
WO2018116688A1