Modified copolymer, rubber composition, resin composition, tire and resin article

A modified copolymer with specific units and a modifying group improves durability and low heat generation, addressing the inadequacies of existing rubber materials in demanding applications like tires.

JP7568498B2Active Publication Date: 2024-10-16BRIDGESTONE CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2020206262
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-11
Publication Date
2024-10-16
Estimated Expiration
2040-12-11

AI Technical Summary

Technical Problem

Existing rubber materials, such as those described in Patent Document 1, do not adequately meet the increasing demand for low heat build-up performance in durable rubber products like tires and other applications.

Method used

A modified copolymer comprising a conjugated diene unit, a non-conjugated olefin unit, and an aromatic vinyl unit, with an alkylstyrene unit and a modifying group containing a carbonyl or thiocarbonyl moiety, is introduced to enhance filler affinity and improve low heat generation properties.

Benefits of technology

The modified copolymer exhibits high durability and excellent low heat generation properties, enhancing the performance of rubber and resin compositions, particularly in tire applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568498000001
    Figure 0007568498000001
Patent Text Reader

Abstract

To provide a copolymer that can express high durability and sufficiently low heat-generating properties.SOLUTION: A modified copolymer has conjugated diene units, non-conjugated olefin units and aromatic vinyl units, the copolymer being free of butylene units. The aromatic vinyl units include alkyl styrene units. The aromatic vinyl units each have a modifying group having a carbonyl moiety (-C(=O)-) and / or a thiocarbonyl moiety (-C(=S)-) bonded thereto.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a modified copolymer, a rubber composition, a resin composition, a tire, and a resin article. [Background technology]

[0002] In general, durability is required for rubber products such as tires, conveyor belts, rubber crawlers, hoses, vibration-isolating rubber used in vibration-isolating devices, and seismic isolation rubber used in seismic isolation devices, and in order to satisfy such requirements, rubber materials with high durability are used.

[0003] As such a highly durable rubber material, for example, Patent Document 1 discloses a multicomponent copolymer having conjugated diene units, non-conjugated olefin units, and aromatic vinyl units, and discloses that the use of this multicomponent copolymer in rubber products can improve durability such as crack growth resistance. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2015 / 190072 Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, the performance requirements for the above-mentioned various rubber products have become increasingly strict, and low heat buildup is being sought as an additional performance requirement. However, the multicomponent copolymer described in Patent Document 1 above may not be sufficient to meet these requirements, and further improvement in low heat buildup is desired.

[0006] Therefore, an object of the present invention is to provide a copolymer that can exhibit excellent low heat buildup properties as well as high durability. Another object of the present invention is to provide a rubber composition, a resin composition, a tire, and a resin article each containing the copolymer. [Means for solving the problem]

[0007] As a result of extensive research, the present inventors have found that a copolymer modified in a specific manner, i.e., a modified copolymer, brings about an improvement in low heat buildup, and have thus completed the present invention.

[0008] The gist and configuration of the present invention to solve the above problems is as follows.

[0009] The copolymer of the present invention is a modified copolymer which has a conjugated diene unit, a non-conjugated olefin unit and an aromatic vinyl unit, but does not have a butylene unit, The aromatic vinyl unit comprises an alkylstyrene unit, The aromatic vinyl unit is characterized in that a modifying group having at least one of a carbonyl moiety (-C(=O)-) and a thiocarbonyl moiety (-C(=S)-) is bonded to the aromatic vinyl unit. The modified copolymer of the present invention can exhibit high durability and excellent low heat buildup.

[0010] In the modified copolymer of the present invention, the aromatic vinyl unit preferably contains a p-methylstyrene unit, which can further improve the affinity of the copolymer with the filler.

[0011] In the modified copolymer of the present invention, the proportion of the conjugated diene units is preferably 10 mol % or more and 80 mol % or less, which can sufficiently improve elongation and strength, improve weather resistance, and, in combination with other units, tend to improve durability and low heat buildup.

[0012] In the modified copolymer of the present invention, the proportion of the non-conjugated olefin units is preferably 10 mol % or more and 80 mol % or less, which improves the weather resistance of the composition and the like, the fracture properties (particularly the breaking strength (Tb)), and the fracture properties at high temperatures (particularly the breaking elongation (Eb)) of the rubber composition and the like, and also improves durability and low heat buildup by combining with other units.

[0013] In the modified copolymer of the present invention, the proportion of the aromatic vinyl units is preferably 0.1 mol % or more and 20 mol % or less, which improves durability such as fracture properties at high temperatures of the rubber composition, and in combination with other units, tends to improve durability as well as low heat buildup.

[0014] The modified copolymer of the present invention preferably has a crystallinity of 0.5% or more and 30% or less, which further improves crack resistance and strength, improves workability during kneading, and improves the tackiness of the modified copolymer.

[0015] In the modified copolymer of the present invention, from the viewpoint of manufacturability and more effectively improving low heat buildup, the modifying group preferably has at least one of an ester bond (-C(=O)O-) and a dithioester bond (-C(=S)S-).

[0016] In the modified copolymer of the present invention, from the viewpoint of productivity and more effectively improving low heat buildup, the modifying group is preferably a group represented by -C(=O)OM or -C(=S)SM (M is an alkali metal atom).

[0017] The modified copolymer of the present invention preferably has a proportion of the modifying groups of 0.1% by mass or more and 10.0% by mass or less, which sufficiently enhances affinity, more reliably exhibits high durability and excellent low heat buildup, and also sufficiently suppresses gelation due to reactions between the modifying groups.

[0018] The rubber composition of the present invention is characterized by containing a rubber component containing the modified copolymer described above. The rubber composition of the present invention has high durability and excellent low heat buildup.

[0019] The rubber composition of the present invention preferably further contains a filler, which can further improve durability, reinforcement, etc.

[0020] The resin composition of the present invention is characterized by containing the modified copolymer described above. By combining the modified copolymer with other resin components, the inherent properties of the other resin components, such as durability and impact resistance, are improved.

[0021] The tire of the present invention is characterized by using the rubber composition described above, and has high durability and low heat buildup.

[0022] The resin article of the present invention is characterized by using the resin composition described above, and has high durability and low heat buildup. [Effects of the Invention]

[0023] According to the present invention, it is possible to provide a copolymer that can exhibit excellent low heat buildup properties as well as high durability. Furthermore, according to the present invention, it is possible to provide a rubber composition, a resin composition, a tire, and a resin article each containing the copolymer. DETAILED DESCRIPTION OF THE INVENTION

[0024] The present invention will be described in detail below based on embodiments.

[0025] (modified copolymer) A modified copolymer according to one embodiment of the present invention (hereinafter, sometimes referred to as "the modified copolymer according to the present embodiment") is a copolymer having conjugated diene units, non-conjugated olefin units, and aromatic vinyl units, but having no butylene units, characterized in that the aromatic vinyl units contain alkylstyrene units, and a modifying group having at least one of a carbonyl moiety (-C(=O)-) and a thiocarbonyl moiety (-C(=S)-) is bonded to the aromatic vinyl units.

[0026] The modified copolymer of this embodiment is obtained by bonding a specific modifying group to the polymer chain of a copolymer having conjugated diene units, non-conjugated olefin units, and aromatic vinyl units. Conventional copolymers having conjugated diene units, non-conjugated olefin units, and aromatic vinyl units have been able to exhibit high durability, but when used in rubber compositions, in particular, there is a demand for further improvement in low heat buildup performance in relation to affinity with fillers such as carbon black and silica contained in the rubber composition. In contrast, in this embodiment, it has been discovered that by adding a specific modifying group that has affinity with fillers to the polymer chain of the copolymer, the affinity of the resulting copolymer with fillers is improved, resulting in high durability and excellent low heat buildup. Furthermore, even when used in a resin composition, the modified copolymer of this embodiment can exhibit high durability and excellent low heat buildup.

[0027] Furthermore, what is particularly noteworthy about the modified copolymer of this embodiment is that at least a portion of the aromatic vinyl units are alkylstyrene units, and a predetermined modifying group is bonded to the aromatic vinyl units. Therefore, in this embodiment, unlike grafting (graft polymerization), modification can be achieved without consuming the double bonds in the main chain of the polymer. As a result, the modified copolymer of this embodiment has the advantage that the effect of having the above-mentioned modifying group can be well exhibited without reducing the effect of having a conjugated diene unit (especially a conjugated diene unit having a double bond in the main chain).

[0028] Here, the conjugated diene unit is a unit that enables vulcanization of the copolymer and can improve the elongation and strength of the rubber. Furthermore, the non-conjugated olefin unit is a unit that can improve durability such as fracture properties by dissipating energy due to the collapse of crystalline components derived from the non-conjugated olefin unit when greatly distorted. Furthermore, the aromatic vinyl unit is a unit that can improve the workability of the copolymer. By combining these units, the modified copolymer of this embodiment can exhibit particularly excellent performance in terms of durability such as fracture properties when used in a rubber composition or a resin composition.

[0029] The conjugated diene unit is a structural unit derived from a conjugated diene compound as a monomer. Here, the conjugated diene compound refers to a conjugated diene compound. The conjugated diene compound preferably has 4 to 8 carbon atoms, and specific examples of such conjugated diene compounds include 1,3-butadiene, isoprene, 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene. The conjugated diene compound may be a single compound or a combination of two or more compounds. From the viewpoint of effectively improving the durability of a composition using the resulting copolymer, the conjugated diene compound as a monomer for the modified copolymer preferably contains at least one compound selected from 1,3-butadiene and isoprene, more preferably consists of at least one compound selected from 1,3-butadiene and isoprene, and even more preferably consists of only 1,3-butadiene. In other words, the conjugated diene units in the modified copolymer preferably contain at least one selected from 1,3-butadiene units and isoprene units, more preferably consist of at least one selected from 1,3-butadiene units and isoprene units, and even more preferably consist of 1,3-butadiene units. Furthermore, such conjugated diene units, when combined with other units, tend to improve durability and low heat buildup.

[0030] The proportion of conjugated diene units in the modified copolymer is preferably 10 mol% or more and 80 mol% or less. If it is 10 mol% or more, elongation and strength can be sufficiently improved. If it is 80 mol% or less, weather resistance can be improved, and in combination with other units, durability and low heat buildup can be easily improved. From the same viewpoint, the proportion of conjugated diene units in the modified copolymer is more preferably 20 mol% or more, even more preferably 25 mol% or more, and more preferably 70 mol% or less, even more preferably 65 mol% or less. The proportion of units such as conjugated diene units in the modified copolymer is substantially the same as the proportion of units such as conjugated diene units in the corresponding copolymer before modification.

[0031] The non-conjugated olefin unit is a structural unit derived from a non-conjugated olefin compound as a monomer. Here, the non-conjugated olefin compound refers to an aliphatic unsaturated hydrocarbon compound having one or more carbon-carbon double bonds. The non-conjugated olefin compound preferably has 2 to 10 carbon atoms. Specific examples of such non-conjugated olefin compounds include α-olefins such as ethylene, propylene, 1-pentene, 1-hexene, 1-heptene, and 1-octene, and heteroatom-substituted alkene compounds such as vinyl pivalate, 1-phenylthioethene, and N-vinylpyrrolidone. The non-conjugated olefin compound may be a single compound or a combination of two or more compounds. From the viewpoint of further improving the weather resistance of compositions using the resulting copolymer, the non-conjugated olefin compound as a monomer for the modified copolymer is preferably an acyclic non-conjugated olefin compound. Furthermore, the acyclic non-conjugated olefin compound is more preferably an α-olefin, even more preferably an α-olefin containing ethylene, and particularly preferably consisting of ethylene alone. In other words, the non-conjugated olefin unit in the modified copolymer is preferably an acyclic non-conjugated olefin unit, and the acyclic non-conjugated olefin unit is more preferably an α-olefin unit, further preferably an α-olefin unit containing an ethylene unit, and particularly preferably composed of only an ethylene unit. Furthermore, when such a non-conjugated olefin unit is used in combination with other units, it is likely to improve durability and low heat buildup.

[0032] The proportion of non-conjugated olefin units in the modified copolymer is preferably 10 mol% or more and 80 mol% or less. If it is 10 mol% or more, the proportion of conjugated diene units or aromatic vinyl units decreases, improving the weather resistance of the composition and improving the fracture properties (particularly, breaking strength (Tb)). If it is 80 mol% or less, the proportion of conjugated diene units or aromatic vinyl units increases, improving the fracture properties (particularly, breaking elongation (Eb)) at high temperatures of the rubber composition. Furthermore, by combining with other units, durability and low heat buildup are likely to be improved. From the same viewpoint, the proportion of non-conjugated olefin units in the modified copolymer is more preferably 20 mol% or more, even more preferably 25 mol% or more, and more preferably 70 mol% or less, even more preferably 65 mol% or less.

[0033] The aromatic vinyl unit is a structural unit derived from an aromatic vinyl compound as a monomer. Here, the term "aromatic vinyl compound" refers to an aromatic compound substituted with at least a vinyl group and is not included in conjugated diene compounds. The modified copolymer of this embodiment must contain at least an alkylstyrene unit as the aromatic vinyl unit from the viewpoint of manufacturability. In other words, at least an alkylstyrene is used as the aromatic vinyl compound used as a monomer. By using an alkylstyrene as a monomer of the modified copolymer, a predetermined modifying group can be easily introduced in large amounts during the production of the modified copolymer. Examples of alkylstyrenes include methylstyrenes such as α-methylstyrene, o-methylstyrene (2-methylstyrene), m-methylstyrene (3-methylstyrene), and p-methylstyrene (4-methylstyrene); o,p-dimethylstyrene; and ethylstyrenes such as o-ethylstyrene, m-ethylstyrene, and p-ethylstyrene. The alkylstyrene unit (and alkylstyrene as a monomer) may be a single type or a combination of two or more types. When a modifying group is introduced into a copolymer having alkylstyrene units, it is thought that the modifying group is preferentially introduced to the primary carbon atom (terminal carbon atom) of the alkyl portion of the alkylstyrene unit.

[0034] In particular, in the modified copolymer of this embodiment, the aromatic vinyl unit preferably contains a p-methylstyrene unit. The methyl group portion of the p-methylstyrene unit contributes less steric hindrance to the copolymer than the main chain portion of the copolymer, so that the modifying group can be introduced more easily and in larger amounts, thereby further improving the affinity of the copolymer with the filler.

[0035] The modified copolymer of this embodiment may have an aromatic vinyl unit other than an alkylstyrene unit (e.g., a styrene unit) as the aromatic vinyl unit. However, from the viewpoint of more fully obtaining the above-mentioned effect, in the modified copolymer of this embodiment, the proportion of alkylstyrene units in the aromatic vinyl units is preferably 80% or more, more preferably 90% or more, and even more preferably 100% (i.e., the aromatic vinyl units are composed only of alkylstyrene units). In other words, the proportion of alkylstyrenes in the aromatic vinyl compound used as a monomer is preferably 80% or more, more preferably 90% or more, and even more preferably 100% (i.e., the aromatic vinyl compound as a monomer is composed only of alkylstyrenes).

[0036] The aromatic ring in the aromatic vinyl unit is not included in the main chain of the copolymer unless it is bonded to an adjacent unit.

[0037] The proportion of aromatic vinyl units in the modified copolymer is preferably 0.1 mol% or more and 20 mol% or less. If it is 0.1 mol% or more, durability such as fracture properties at high temperatures of rubber compositions and the like is improved. Furthermore, if it is 20 mol% or less, the effects of the conjugated diene units and non-conjugated olefin units become significant, and further, by combining with other units, durability and low heat buildup are likely to be improved. From the same viewpoint, the proportion of aromatic vinyl units in the modified copolymer is more preferably 0.3 mol% or more, even more preferably 0.5 mol% or more, and more preferably 10 mol% or less, even more preferably 5 mol% or less.

[0038] In order to reliably obtain the desired effects, the modified copolymer does not contain a butylene unit, i.e., it is preferable that the modified copolymer does not contain, for example, a polymer obtained by hydrogenating butadiene or a hydrogenated product of a styrene-butadiene copolymer such as styrene-ethylene / butylene-styrene (SEBS).

[0039] The modified copolymer may have other structural units in addition to the conjugated diene units, non-conjugated olefin units, and aromatic vinyl units. However, from the viewpoint of obtaining the desired effect, the proportion of the other structural units in the entire copolymer is preferably 30 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, and particularly preferably 0 mol% (i.e., the modified copolymer consists only of conjugated diene units, non-conjugated olefin units, and aromatic vinyl units).

[0040] The modified copolymer preferably has a weight average molecular weight (Mw) of 10,000 or more and 10,000,000 or less in terms of polystyrene. Having an Mw of 10,000 or more ensures sufficient mechanical strength, while having an Mw of 10,000,000 or less ensures high workability. From the same viewpoint, the Mw of the modified copolymer is more preferably 100,000 or more, even more preferably 150,000 or more, and more preferably 9,000,000 or less, even more preferably 8,000,000 or less.

[0041] The modified copolymer preferably has a polystyrene-equivalent number average molecular weight (Mn) of 10,000 or more and 10,000,000 or less. Having an Mn of 10,000 or more ensures sufficient mechanical strength, while having an Mn of 10,000,000 or less maintains high workability. From the same viewpoint, the Mn of the modified copolymer is more preferably 50,000 or more, even more preferably 100,000 or more, and more preferably 9,000,000 or less, even more preferably 8,000,000 or less.

[0042] The molecular weight distribution [Mw / Mn (weight average molecular weight / number average molecular weight)] of the modified copolymer is preferably 1.00 or more and 4.00 or less. If the molecular weight distribution of the modified copolymer is 4.00 or less, sufficient homogeneity in the physical properties of the modified copolymer can be achieved. From the same viewpoint, the molecular weight distribution of the modified copolymer is more preferably 3.50 or less, and even more preferably 3.00 or less. Furthermore, the molecular weight distribution of the modified copolymer is more preferably 1.50 or more, and even more preferably 1.80 or more.

[0043] The weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) are determined by gel permeation chromatography (GPC) using polystyrene as a standard substance.

[0044] The modified copolymer preferably has a melting point of 30°C or higher, and preferably 180°C or lower, as measured by differential scanning calorimetry (DSC). If the melting point of the modified copolymer is 30°C or higher, the crystallinity of the modified copolymer is increased, further improving crack resistance. If the melting point is 180°C or lower, there is no need to excessively increase the heating temperature during heating, further improving workability. From the same viewpoint, the melting point of the modified copolymer is more preferably 140°C or lower. If the copolymer has two or more melting points, the highest melting point is used.

[0045] The modified copolymer preferably has a crystallinity (ΔH / ΔH0×100, also referred to as "crystalline amount") of 0.5% or more, and preferably 30% or less. When the modified copolymer has a crystallinity of 0.5% or more, the crystallinity resulting from the non-conjugated olefin units is sufficiently ensured, further improving crack resistance and strength. When the modified copolymer has a crystallinity of 30% or less, workability during kneading and the like is improved, and the tackiness of the modified copolymer is also improved, thereby improving workability, for example, when rubber members made from the rubber composition are attached to each other to form rubber articles such as tires. From the same viewpoint, the crystallinity of the modified copolymer is more preferably 1% or more, even more preferably 1.5% or more, and more preferably 25% or less, even more preferably 20% or less. The degree of crystallinity can be determined as the ratio (ΔH / ΔH × 100) of the endothermic peak energy (ΔH) of the copolymer to the crystalline melting energy (ΔH) of 100% crystalline polyethylene, measured with a differential scanning calorimeter (DSC). The crystalline heat of fusion (crystalline melting energy) of polyethylene is 293 J / g.

[0046] The main chain of the modified copolymer may have a cyclic structure, or the main chain may consist of only an acyclic structure. When the main chain consists of only an acyclic structure, the abrasion resistance of the rubber composition and the like and the durability after crosslinking can be further improved. In addition, it becomes easier to introduce a predetermined modifying group into the copolymer. Note that NMR is used as the main measurement means to confirm whether the main chain of the copolymer has a cyclic structure. Specifically, peaks derived from the cyclic structure present in the main chain (for example, for three- to five-membered rings, 13 When the peak (which appears at 10 to 24 ppm in a C-NMR spectrum chart) is not observed, it indicates that the main chain of the copolymer is composed of only acyclic structures. On the other hand, when the peak is observed, it indicates that the main chain of the copolymer has a cyclic structure.

[0047] The modified copolymer of this embodiment can be preferably produced by introducing a modifying group into a predetermined position of an (unmodified) copolymer having a conjugated diene unit, a non-conjugated olefin unit, and an aromatic vinyl unit. In this case, for example, the copolymer described in WO2017 / 065301A1 can be preferably used as the (unmodified) copolymer having a conjugated diene unit, a non-conjugated olefin unit, and an aromatic vinyl unit.

[0048] The modified copolymer of this embodiment has a modifying group having at least one of a carbonyl moiety (-C(=O)-) and a thiocarbonyl moiety (-C(=S)-), and the modifying group is bonded to an aromatic vinyl unit in the copolymer. From the viewpoints of manufacturability and more effectively improving low heat buildup, the modifying group preferably has at least one of an ester bond (-C(=O)O-) and a dithioester bond (-C(=S)S-). Examples of such modifying groups include groups corresponding to carboxylates, i.e., -C(=O)OR (where R is any group), and groups corresponding to dithiocarboxylates, i.e., -C(=S)SR (where R is any group). Furthermore, from the viewpoints of manufacturability and more effectively improving low heat buildup, the modifying group is more preferably a group represented by -C(=O)OM or -C(=S)SM (where M is an alkali metal atom). In short, such a modifying group is a group corresponding to a metal carboxylate or a metal dithiocarboxylate.

[0049] In the modified copolymer of this embodiment, the above-mentioned modifying group may be further bonded to any position other than the alkylstyrene unit.

[0050] The method for producing such a modified copolymer is not particularly limited, and examples thereof include a method comprising the steps of: (i) adding an alkali metal compound to an (unmodified) copolymer having conjugated diene units, non-conjugated olefin units, and aromatic vinyl units containing at least alkylstyrene units, but no butylene units; and (ii) reacting the product obtained in step (i) with a predetermined modifying agent to introduce a modifying group into the copolymer.

[0051] As described above, the copolymer before modification can be prepared, for example, according to the method described in WO2017 / 065301A1.

[0052] Examples of the alkali metal atom (M) of the alkali metal compound added in the above step (i) include Li, Na, K, Rb, and Cs. Examples of the alkali metal compound include organic alkali metal compounds and organic alkaline earth metal compounds. The alkali metal compound is preferably an organic alkali metal compound.

[0053] Organoalkali metal compounds include, for example, hydrocarbyl lithium and lithium amide compounds.

[0054] The hydrocarbyllithium is preferably, for example, one having a hydrocarbyl group having 2 to 20 carbon atoms, and examples thereof include ethyllithium, n-propyllithium, isopropyllithium, n-butyllithium, isobutyllithium, sec-butyllithium, tert-butyllithium, tert-octyllithium, n-decyllithium, phenyllithium, 2-naphthyllithium, 2-butylphenyllithium, 4-phenylbutyllithium, cyclohexyllithium, cyclopentyllithium, and a reaction product of diisopropenylbenzene with butyllithium.

[0055] Examples of lithium amide compounds include lithium hexamethyleneimide, lithium pyrrolidide, lithium piperidide, lithium heptamethyleneimide, lithium dodecamethyleneimide, lithium dimethylamide, lithium diethylamide, lithium dibutylamide, lithium dipropylamide, lithium diheptylamide, lithium dihexylamide, lithium dioctylamide, lithium di-2-ethylhexylamide, lithium didecylamide, lithium-N-methylpiberazide, lithium ethylpropylamide, lithium ethylbutylamide, lithium ethylbenzylamide, and lithium methylphenethylamide.

[0056] From the viewpoint of more efficiently introducing the modifying group into the copolymer, the alkali metal compound used in step (i) is preferably sec-butyllithium.

[0057] By adding an alkali metal compound in step (i), alkali metal atoms are introduced into a portion of the polymer main chain of the copolymer other than one end (e.g., in the middle of the polymer main chain) (hydrogen atoms in the hydrocarbon chain are substituted with alkali metal atoms), and the introduced alkali metal atoms react with the modifying agent to introduce a modifying group.

[0058] Examples of the portion into which the alkali metal atom is introduced in step (i) include the tertiary carbon atom at the bond between the alkylstyrene unit and the polymer main chain and the primary carbon atom (terminal carbon atom) of the alkyl portion. However, in this case, the alkali metal atom is presumably preferentially introduced into the primary carbon atom because the primary carbon atom has less steric hindrance than the tertiary carbon atom.

[0059] Examples of the modifying agent used in step (ii) include carbon dioxide and carbon disulfide. In particular, the use of carbon dioxide makes it easier to introduce the modifying group. When carbon dioxide is used as the modifying agent, the modifying group introduced into the copolymer can be -C(=O)OM (M is an alkali metal atom). When carbon disulfide is used as the modifying agent, the modifying group introduced into the copolymer can be -C(=S)SM (M is an alkali metal atom).

[0060] Furthermore, another method for producing a modified copolymer includes a method in which a modifying group is previously added to any of basic monomers such as conjugated diene compounds, non-conjugated olefin compounds, and aromatic vinyl compounds including alkylstyrenes, and the resulting monomer is then copolymerized.

[0061] The proportion of the modifying group in the modified copolymer is preferably 0.1% by mass or more and 10.0% by mass or less. If the proportion of the modifying group is 0.1% by mass or more, affinity is sufficiently increased, and high durability and excellent low heat buildup can be more reliably achieved. Furthermore, if the proportion of the modifying group is 10.0% by mass or less, gelation due to reaction between the modifying groups can be sufficiently suppressed. The above proportion is not limited to the modifying group bonded to the alkylstyrene unit, but refers to the proportion of the modifying group present in the modified copolymer. From the same perspective, the proportion of the modifying group in the modified copolymer is more preferably 0.3% by mass or more, even more preferably 0.5% by mass or more, even more preferably 1.0% by mass or more, and more preferably 7.0% by mass or less, even more preferably 5.0% by mass or less, and even more preferably 3.0% by mass or less. The proportion of modifying groups in the modified copolymer can be increased, for example, by increasing the amount of modifier added, increasing the amount of the alkali metal compound added, increasing the amount of aromatic vinyl units in the copolymer, or further increasing the amount of alkylstyrene units as aromatic vinyl units. The proportion of the modifying group in the modified copolymer is 1 It can be calculated from the H-NMR spectrum.

[0062] The modified copolymer of this embodiment exhibits high durability and low heat buildup, and is therefore suitable for use in the rubber compositions and resin compositions described below. In particular, since the rubber composition using the modified copolymer of this embodiment exhibits high durability and low heat buildup, it is suitable for use in rubber products such as tires, conveyor belts, rubber crawlers, hoses, vibration-isolating rubber used in vibration-isolating devices, and seismic isolation rubber used in seismic isolation devices.

[0063] (Rubber composition) A rubber composition according to one embodiment of the present invention (hereinafter sometimes referred to as "the rubber composition of the present embodiment") contains a rubber component including the modified copolymer described above. Because the rubber composition of the present embodiment contains the modified copolymer described above, it has high durability and excellent low heat buildup.

[0064] The rubber composition of this embodiment may contain rubber components other than the modified copolymer described above. Examples of other rubber components include natural rubber (NR), such as high-purity natural rubber, epoxidized natural rubber, hydroxylated natural rubber, hydrogenated natural rubber, and modified natural rubber (e.g., grafted natural rubber), as well as RSS and TSR; butadiene rubber (BR); isoprene rubber (IR); styrene-butadiene rubber (SBR); styrene-isoprene-butadiene rubber (SIBR); butyl rubber; ethylene-propylene rubber (EPM); ethylene propylene diene rubber (EPDM); chloroprene rubber (CR); acrylonitrile butadiene rubber (NBR); polysulfide rubber; silicone rubber; fluororubber; and urethane rubber. These other rubber components may be used singly or in combination of two or more.

[0065] The butadiene rubber (BR) may contain high-cis polybutadiene rubber in consideration of improving abrasion resistance. The high-cis polybutadiene rubber is a high-cis polybutadiene rubber having a cis-1,4 bond content in 1,3-butadiene units of 90% to 99% as measured by FT-IR. The cis-1,4 bond content in 1,3-butadiene units of the high-cis polybutadiene rubber is preferably 95% to 99%.

[0066] The method for producing high-cis polybutadiene rubber is not particularly limited, and it may be produced by a known method, for example, a method of polymerizing butadiene using a neodymium-based catalyst. High-cis polybutadiene rubber is also commercially available, for example, "BR01" and "T700" (both manufactured by JSR Corporation), and "Ubepol BR150L" (manufactured by Ube Industries, Ltd.).

[0067] From the viewpoint of reliably achieving the effects of expressing durability and low heat buildup, the proportion of the modified copolymer of this embodiment in the rubber component is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 100% by mass, i.e., the entire amount is the modified copolymer.

[0068] The rubber composition of this embodiment preferably further contains a filler. By including a filler, durability, reinforcement, and the like can be further improved. Examples of fillers include silica, carbon black, aluminum oxide, clay, alumina, talc, mica, kaolin, glass balloons, glass beads, calcium carbonate, magnesium carbonate, magnesium hydroxide, calcium carbonate, magnesium oxide, titanium oxide, potassium titanate, and barium sulfate. One type of filler may be used alone, or two or more types may be used in combination. From the viewpoint of improving dispersibility in the modified copolymer, the filler preferably contains at least one type selected from silica and carbon black.

[0069] The carbon black is not particularly limited, and examples thereof include SAF, ISAF, HAF, FF, FEF, GPF, SRF, CF, FT, and MT grade carbon black. One type of carbon black may be used alone, or two or more types may be used in combination. Among these, SAF, ISAF, and HAF grade carbon black are preferred.

[0070] The silica is not particularly limited, and examples thereof include wet silica, dry silica, and colloidal silica. Silica may be used alone or in combination of two or more. Among these, wet silica is preferred.

[0071] The content of the filler in the rubber composition of the present embodiment is preferably 30 to 100 parts by mass per 100 parts by mass of the rubber component. When the content is 30 parts by mass or more, durability and abrasion resistance can be further improved, and when the content is 100 parts by mass or less, low loss properties and high elastic modulus can be well maintained.

[0072] When silica is used as a filler, the rubber composition of this embodiment preferably contains a silane coupling agent to improve the compounding effect of the silica. Examples of silane coupling agents include vinyltriethoxysilane, vinyltris(β-methoxyethoxy)silane, γ-methacryloxypropyltrimethoxysilane, vinyltriacetoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-chloropropylmethoxysilane, vinyltrichlorosilane, γ-mercaptopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, bis-triethoxysilylpropyltetrasulfide, and bis-triethoxysilylpropyldisulfide. These silane coupling agents may be used alone or in combination of two or more.

[0073] The content of the silane coupling agent is not particularly limited, but is preferably 1 to 12 mass %, more preferably 3 to 10 mass %, relative to the content of silica as a filler. When the content of the silane coupling agent is 1 mass % or more relative to the content of silica as a filler, the effect of improving the dispersibility of the filler is easily obtained, and when it is 12 mass % or less, the incorporation of an excessive amount of the silane coupling agent is suppressed, and the addition effect can be obtained efficiently, which is also economically advantageous.

[0074] Furthermore, the rubber composition of the present embodiment may contain, as needed, components such as a crosslinking agent (including a vulcanizing agent such as sulfur), a crosslinking accelerator (vulcanization accelerator), a crosslinking acceleration aid (vulcanization acceleration aid), an antioxidant, zinc oxide (ZnO), a softener, waxes, an antioxidant, a foaming agent, a plasticizer, a lubricant, a tackifier, a petroleum-based resin, an ultraviolet absorber, a dispersant, a compatibilizer, and a homogenizer, as long as the effects of the present invention are not impaired.

[0075] The rubber composition of the present embodiment has high durability and low heat buildup, and is therefore suitable for use in rubber products such as tires, which will be described later, conveyor belts, rubber crawlers, hoses, vibration-isolating rubber used in vibration-isolating devices, and seismic isolation rubber used in seismic isolation devices.

[0076] The method for producing the rubber composition of this embodiment is not particularly limited, and can be, for example, produced by kneading the above-mentioned components using a kneading machine such as a Banbury mixer, roll, or internal mixer. Here, during blending and kneading, all components may be blended and kneaded at once, or each component may be blended and kneaded in multiple stages, such as two or three stages. For kneading, a kneading machine such as a roll, internal mixer, or Banbury rotor can be used. Furthermore, when molding the rubber composition into a sheet or strip, a known molding machine such as an extruder or press can be used.

[0077] The rubber composition of the present embodiment may be produced by crosslinking (vulcanization). The crosslinking conditions are not particularly limited, and typically a temperature of 140 to 180° C. and a time of 5 to 120 minutes can be used.

[0078] (Resin composition and resin article) A resin composition according to one embodiment of the present invention contains the modified copolymer described above. By combining the modified copolymer with other resin components, the inherent properties of the other resin components, such as durability and impact resistance, are improved. Furthermore, a resin article according to one embodiment of the present invention uses the resin composition described above. The resin article has high durability and low heat buildup.

[0079] The resin component to be combined with the modified copolymer is not particularly limited, and various resin components can be used, and may be appropriately selected depending on the performance desired for the resin article. Examples of such resin components include homopolymers such as polyethylene, polypropylene, polybutene, and polystyrene, copolymers such as ethylene-propylene copolymer, ethylene-methacrylic acid copolymer, ethylene-ethyl acrylate copolymer, ethylene-propylene-diene terpolymer, and ethylene-vinyl acetate copolymer, and ionomer resins thereof, polyolefin resins such as vinyl alcohol homopolymers and polyvinyl alcohol resins such as ethylene-vinyl alcohol copolymers, poly(meth)acrylic acid resins and their ester resins, polyamide resins such as aliphatic polyamide resins and aromatic polyamide resins, polyethylene glycol resins, carboxyvinyl copolymers, styrene-maleic acid copolymers, polyvinylpyrrolidone resins such as vinylpyrrolidone homopolymers and vinylpyrrolidone-vinyl acetate copolymers, polyester resins, cellulose resins, mercaptomethanol, hydrogenated styrene-butadiene, syndiotactic polybutadiene, trans-polybutadiene, and trans-polyisobutadiene. Among these, the resin component is preferably a polyolefin resin containing a non-conjugated olefin unit contained in a modified copolymer, and more preferably polyethylene, polypropylene, or polybutene.

[0080] In the resin composition, the content of the modified copolymer relative to all resin components may be adjusted appropriately depending on the other resins to be combined, the desired properties, etc., and is usually about 1 to 99 mass %, preferably 5 to 90 mass %.

[0081] The resin composition may contain various additives depending on the desired performance. The various additives are not particularly limited, and additives typically contained in resin compositions may be used, such as weathering agents such as ultraviolet absorbers and light stabilizers, antioxidants, fillers exemplified as fillers that may be contained in the rubber composition, softeners, colorants, flame retardants, plasticizers, and antistatic agents.

[0082] (tire) A tire according to one embodiment of the present invention uses the rubber composition described above. Because the tire uses the rubber composition according to this embodiment, it has high durability and low heat buildup. The application site of the rubber composition of this embodiment in a tire is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include the tread, base tread, sidewall, belt coating rubber, ply coating rubber, side reinforcing rubber, and bead filler. From the viewpoint of effectively utilizing the excellent effects of the rubber composition of this embodiment, namely high durability and low heat buildup, the application site is preferably the tread, and particularly the tread of a studless tire. Furthermore, since the composition is also suitable for use as an adhesive with metal, application to the belt coating rubber is also preferred.

[0083] The tire can be manufactured by a conventional method. For example, components typically used in tire manufacturing, such as a carcass layer, a belt layer, and a tread layer, each composed of the unvulcanized rubber composition of the present embodiment and / or cords, are laminated on a tire-building drum, and the drum is removed to form a green tire. The green tire is then heated and vulcanized in a conventional manner to manufacture a desired tire (e.g., a pneumatic tire).

[0084] (Products other than tires) The rubber composition and resin composition described above can be applied to various rubber articles and resin articles other than tires. For example, the above-described composition can be preferably applied to automobile parts (automobile seats, automobile batteries (lithium ion batteries, etc.), weather strips, hoses, anti-vibration rubbers, cables, sealing materials, etc.). In addition, the above-mentioned compositions can be used in conveyor belts, crawlers, anti-vibration rubber, hoses, resin piping, sound-absorbing materials, bedding, precision parts for office equipment (OA (office automation) rollers), bicycle frames, golf balls, tennis rackets, golf shafts, resin additives, filters, adhesives, pressure-sensitive adhesives, inks, medical devices (medical tubes, bags, microneedles, rubber sleeves, artificial organs, caps, packings, syringe gaskets, medicine stoppers, artificial legs, artificial limbs), cosmetics (UV (ultraviolet) powder, puffs, containers, wax, shampoo, conditioner), detergents, building materials (flooring materials, seismic isolation rubber, seismic isolation rubber, building films, sound-absorbing materials, waterproof sheets, heat insulation materials, joint materials, sealing materials), packaging materials, liquid crystal materials, organic electroluminescence (EL) (electro- The present invention can also be preferably applied to (luminescence) materials, organic semiconductor materials, electronic materials, electronic devices, communication equipment, aircraft parts, machine parts, electronic parts, agricultural materials, electric wires, cables, textiles (wearable bases), daily necessities (toothbrushes, shoe soles, eyeglasses, artificial bait, binoculars, toys, dust masks, garden hoses), robot parts, optical parts, road materials (asphalt, guardrails, poles, signs), protective equipment (shoes, bulletproof vests), exterior parts for electrical equipment, exterior parts for office equipment, soles, sealants, etc. [Example]

[0085] The present invention will be explained in more detail below by way of examples, but the present invention is not limited to the following examples and can be modified as appropriate within the scope of the present invention.

[0086] (Preparation of Modified Copolymer A1) To a thoroughly dried 2000 mL pressure-resistant stainless steel reactor, 16 g of styrene as an aromatic vinyl compound and 364 g of toluene were added. In a glove box under a nitrogen atmosphere, 0.025 mmol of mono(bis(1,3-tert-butyldimethylsilyl)indenyl)bis(bis(dimethylsilyl)amido) gadolinium complex (1,3-[(t-Bu)MeSi]CHGd[N(SiHMe)]), 0.025 mmol of trityl tetrakis(pentafluorophenyl)borate [PhCB(CF)], and 0.75 mmol of triisobutylaluminum were placed in a glass vessel, and 15 mL of toluene was added to prepare a catalyst solution. The catalyst solution was then added to the pressure-resistant stainless steel reactor and heated to 60°C. Next, ethylene as a non-conjugated olefin compound was introduced into the pressure-resistant stainless steel reactor at a pressure of 0.6 MPa, and copolymerization was carried out for 61 minutes at 75° C. Furthermore, 260 g of a toluene solution containing 80 g of 1,3-butadiene as a conjugated diene compound was continuously added at a rate of 4.0 to 7.0 mL / min. Next, 1 mL of a 5% by mass solution of 2,2'-methylene-bis(4-ethyl-6-t-butylphenol) (NS-5) in isopropanol was added to the pressure-resistant stainless steel reactor to terminate the reaction. After separation using a large amount of methanol and vacuum drying at 50°C, copolymer A0 (before the introduction of the modifying group) was obtained. That is, in preparing copolymer A0, no alkylstyrene was used as a monomer.

[0087] 20 g of the copolymer and 380 g of cyclohexane were added to a 1 L glass bottle and stirred in an 80 °C water bath for 2 hours to dissolve the copolymer in cyclohexane. Next, a hexane solution containing 3.4 mmol of sec-butyllithium and 3.4 mmol of tetramethylethylenediamine were added to the glass bottle and reacted at 80 °C for 1 hour. After the reaction, the glass bottle was removed from the water bath, and carbon dioxide (CO2) was bubbled into the reacted solution for 1 minute. The solution was then left to stand overnight at room temperature to complete the modification reaction. The mixture was then separated using a large amount of methanol and vacuum dried at 50 °C to finally obtain copolymer A1 having a modifying group (-C(=O)OLi) (particularly, mainly on the tertiary carbon atom of the bond between the styrene unit and the polymer main chain).

[0088] (Preparation of Modified Copolymer B1) To a thoroughly dried 2000 mL pressure-resistant stainless steel reactor, 7 g of p-methylstyrene as an aromatic vinyl compound and 373 g of toluene were added. In a glove box under a nitrogen atmosphere, 0.025 mmol of mono(bis(1,3-tert-butyldimethylsilyl)indenyl)bis(bis(dimethylsilyl)amido) gadolinium complex (1,3-[(t-Bu)MeSi]CHGd[N(SiHMe)]), 0.025 mmol of trityl tetrakis(pentafluorophenyl)borate [PhCB(CF)], and 0.75 mmol of triisobutylaluminum were placed in a glass vessel, and 15 mL of toluene was added to prepare a catalyst solution. The catalyst solution was then added to the pressure-resistant stainless steel reactor and heated to 60°C. Next, ethylene as a non-conjugated olefin compound was introduced into the pressure-resistant stainless steel reactor at a pressure of 0.6 MPa, and copolymerization was carried out for 117 minutes at 75°C. In addition, 260 g of a toluene solution containing 80 g of 1,3-butadiene as a conjugated diene compound was continuously added at a rate of 2.0 to 4.0 mL / min. Next, 1 mL of a 5% by mass solution of 2,2'-methylene-bis(4-ethyl-6-t-butylphenol) (NS-5) in isopropanol was added to the pressure-resistant stainless steel reactor to terminate the reaction. After separation using a large amount of methanol and vacuum drying at 50°C, copolymer B0 (before the introduction of the modifying group) was obtained.

[0089] 20 g of the copolymer and 380 g of cyclohexane were added to a 1 L glass bottle and stirred in an 80 °C water bath for 2 hours to dissolve the copolymer in cyclohexane. Next, a hexane solution containing 3.4 mmol of sec-butyllithium and 3.4 mmol of tetramethylethylenediamine were added to the glass bottle and reacted at 80 °C for 1 hour. After the reaction, the glass bottle was removed from the water bath, and carbon dioxide (CO2) was bubbled into the reacted solution for 1 minute. The solution was then left to stand overnight at room temperature to complete the modification reaction. The mixture was then separated using a large amount of methanol and vacuum dried at 50 °C to finally obtain copolymer B1 having a modifying group (-C(=O)OLi) (particularly, mainly at the methyl moiety at the 4-position of the p-methylstyrene unit).

[0090] The copolymer was analyzed by gel permeation chromatography (GPC: HLC-8220GPC / HT manufactured by Tosoh Corporation, column: GMH manufactured by Tosoh Corporation). HR The weight average molecular weight (Mw), number average molecular weight (Mn), and molecular weight distribution (Mw / Mn) in terms of polystyrene were determined using a -H(S)HT x 2, detector: differential refractometer (RI) with monodisperse polystyrene as the standard. The measurement temperature was 140°C. The results are shown in Table 1.

[0091] Furthermore, using a differential scanning calorimeter (DSC, manufactured by TA Instruments Japan, "DSCQ2000"), the copolymer was heated from -150°C to 150°C at a rate of 10°C / min, and the endothermic peak energy (ΔH1) from 0°C to 100°C and the endothermic peak energy (ΔH2) from 100°C to 150°C were measured. The crystalline melting energy (ΔH0) of the 100% crystalline polyethylene was used to calculate the crystallinity of the copolymer from 0°C to 100°C and from 100°C to 150°C, respectively, based on the ratio of the endothermic peak energy of the copolymer to the crystalline melting energy (ΔH0) of the polyethylene ((ΔH1 / ΔH0) × 100, (ΔH2 / ΔH0) × 100). The results are shown in Table 1. The above crystallinity is the crystallinity in the range of 0 to 150°C. For example, when the crystallinity is described separately for 0 to 100°C and for 100 to 150°C, the sum of these values ​​is the crystallinity for 0 to 150°C.

[0092] The proportions (mol%) of conjugated diene units (1,3-butadiene units), non-conjugated olefins (ethylene units), and aromatic vinyl units (styrene units, p-methylstyrene units) in the copolymer are: 1 The results were calculated from the integral ratio of each peak in the H-NMR spectrum (100°C, d-tetrachloroethane standard: 6 ppm). The results are shown in Table 1.

[0093] The proportion of the modifying group in the copolymer is 1 The results were calculated from the H-NMR spectrum and are shown in Table 1.

[0094] Furthermore, regarding the above copolymer, 13 The C-NMR spectrum was measured. 13 In the C-NMR spectrum chart, no peaks were observed between 10 and 24 ppm, which confirmed that the main chain of each of the synthesized copolymers was composed solely of an acyclic structure.

[0095] [Table 1] [Industrial Applicability]

[0096] According to the present invention, it is possible to provide a copolymer that can exhibit excellent low heat buildup properties as well as high durability. Furthermore, according to the present invention, it is possible to provide a rubber composition, a resin composition, a tire, and a resin article each containing the copolymer.

Claims

1. A modified copolymer having a conjugated diene unit, a non-conjugated olefin unit and an aromatic vinyl unit, and having no butylene unit, The aromatic vinyl unit comprises an alkylstyrene unit, a modifying group having at least one of a carbonyl moiety (-C(=O)-) and a thiocarbonyl moiety (-C(=S)-) is bonded to the alkylstyrene unit; The proportion of the non-conjugated olefin units is 25 mol % or more and 80 mol % or less, The ratio of the conjugated diene units is 10 mol % or more and 65 mol % or less, The ratio of the aromatic vinyl unit is 0.1 mol % or more and 10 mol % or less, The crystallinity is 0.5% or more and 30% or less. A modified copolymer, characterized in that:

2. 2. The modified copolymer of claim 1, wherein the aromatic vinyl units comprise p-methylstyrene units.

3. 3. The modified copolymer according to claim 1, wherein the modifying group comprises at least one of an ester bond (-C(=O)O-) and a dithioester bond (-C(=S)S-).

4. The modified copolymer according to any one of claims 1 to 3, wherein the modifying group is a group represented by -C(=O)OM or -C(=S)SM (M is an alkali metal atom).

5. The modified copolymer according to any one of claims 1 to 4, wherein the proportion of the modifying group is 0.1% by mass or more and 10.0% by mass or less.

6. A rubber composition comprising a rubber component containing the modified copolymer according to any one of claims 1 to 5.

7. The rubber composition according to claim 6, further comprising a filler.

8. A resin composition comprising the modified copolymer according to any one of claims 1 to 5.

9. A tire comprising the rubber composition according to claim 6 or 7.

10. A resin article, comprising the resin composition according to claim 8.

Citation Information

Patent Citations

  • Manufacturing method of multi-component copolymer and multi-component copolymer

    JP2017101181A

  • Multi-component copolymer, rubber composition, and tire

    WO2015190072A1

  • Modified conjugated diene polymer, rubber composition, tire, and method for manufacturing modified conjugated diene polymer

    WO2019045053A1

  • Rubber composition and tire

    WO2020059367A1