Adhesive sheet

The pressure-sensitive adhesive sheet with controlled adhesive properties addresses fluidity inconsistencies in resin sealing for semiconductor chips, ensuring stable and uniform resin flow for improved sealing quality.

JP7568825B2Active Publication Date: 2024-10-16NITTO DENKO CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023503373
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-03-05
Filing Date
2021-11-01
Publication Date
2024-10-16
Estimated Expiration
2041-11-01

AI Technical Summary

Technical Problem

The fluidity of sealing resin precursors during the resin sealing process for semiconductor chips is inconsistent due to variations in the adhesive layer's surface properties and affinity with the sealing resin, affecting sealing quality and process efficiency.

Method used

A pressure-sensitive adhesive sheet with specific adhesive properties, including a base polymer with an sp value of 7 to 10 (cal/cm³)¹/², moisture content of 0.05% to 6% by weight, and a thickness of 2 to 15 μm, which stabilizes the fluidity of the sealing resin, allowing for uniform resin sealing.

Benefits of technology

The adhesive sheet ensures consistent resin flow with minimal variation, enhancing sealing quality and process efficiency by reducing fluidity inconsistencies and enabling stable, uniform resin sealing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568825000002
    Figure 0007568825000002
  • Figure 0007568825000003
    Figure 0007568825000003
  • Figure 0007568825000004
    Figure 0007568825000004
Patent Text Reader

Abstract

The present invention provides an adhesive sheet including, on the surface thereof, an adhesive layer on which a sealing resin for sealing a semiconductor chip can evenly flow. An adhesive sheet according to the present invention includes a substrate and an adhesive layer that is disposed on at least one side of the substrate, wherein the adhesive force at 23°C when the adhesive layer is bonded to polyethylene terephthalate is 0.1N / 20mm to 8N / 20mm, the adhesive layer is composed of an adhesive that contains a base polymer, the sp value of the base polymer is 7(cal / cm3)1 / 2 to 10(cal / cm3)1 / 2, and the water content of the adhesive sheet is 0.05wt% to 6wt%.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive sheet. [Background technology]

[0002] In recent years, in the manufacture of semiconductor parts including semiconductor chips, the semiconductor chips are sometimes resin-sealed to prevent the semiconductor chips from being scratched, expand metal wiring, etc. In the resin sealing process, the semiconductor chips are sometimes resin-sealed on an adhesive sheet from the viewpoint of workability, etc. For example, in order to prevent the semiconductor chips from moving, multiple semiconductor chips are placed on an adhesive sheet as a predetermined temporary fixing material, and the semiconductor chips are collectively sealed on the adhesive sheet.

[0003] In the resin encapsulation process, a semiconductor chip is covered with a fluid encapsulation resin precursor, and then the fluidity of the precursor is reduced to encapsulate the semiconductor chip. The fluidity of the precursor at this time is one of the factors that affect the encapsulation quality (particularly, the working time and the uniformity of encapsulation). In general, the fluidity of the precursor depends on the affinity between the surface to which the encapsulation resin is applied (i.e., the surface of the adhesive layer of the adhesive sheet) and the encapsulation resin. However, even if there is no change in the composition of the adhesive layer and the encapsulation resin, the fluidity of the precursor may not be constant. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2001-308116 A [Patent Document 2] JP 2001-313350 A Summary of the Invention [Problem to be solved by the invention]

[0005] The present invention has been made to solve the above-mentioned problems in the conventional art, and an object of the present invention is to provide an adhesive sheet having an adhesive layer on its surface which allows the sealing resin that seals semiconductor chips, etc. to flow with little variation. [Means for solving the problem]

[0006] The pressure-sensitive adhesive sheet of the present invention is a pressure-sensitive adhesive sheet comprising a substrate and a pressure-sensitive adhesive layer disposed on at least one side of the substrate, the pressure-sensitive adhesive layer having an adhesive strength of 0.1 N / 20 mm to 8 N / 20 mm at 23° C. when attached to polyethylene terephthalate, the pressure-sensitive adhesive layer being made of a pressure-sensitive adhesive containing a base polymer, the base polymer having an sp value of 7 (cal / cm 3 ) 1 / 2 ~10(cal / cm 3 ) 1 / 2 The moisture content of the pressure-sensitive adhesive sheet is 0.05% by weight to 6% by weight. In one embodiment, the substrate is a resin sheet made of a resin having a glass transition temperature (Tg) of 60°C to 450°C. In one embodiment, the substrate is made of an aromatic polyimide resin. In one embodiment, the pressure-sensitive adhesive layer has a thickness of 2 μm to 15 μm. In one embodiment, the pressure-sensitive adhesive layer has a gel fraction of 60% to 100%. In one embodiment, the base polymer is an acrylic polymer, the acrylic polymer contains structural units derived from hydroxyl group-containing monomers, and the content of the structural units derived from hydroxyl group-containing monomers is 0.1 parts by weight to 20 parts by weight per 100 parts by weight of all structural units constituting the acrylic polymer. In one embodiment, the pressure-sensitive adhesive sheet further comprises a second pressure-sensitive adhesive layer on the opposite side of the substrate to the pressure-sensitive adhesive layer. In one embodiment, the pressure sensitive adhesive sheet is used as a sheet for temporarily fixing a semiconductor chip during the manufacture of a CSP (Chip Size / Scale Package) or a WLP (Wafer Level Package). In one embodiment, the semiconductor chip is sealed with a sealing resin, and the processing temperature during the resin sealing is 100° C. or higher. According to another aspect of the present invention, there is provided a method for producing the above-mentioned pressure-sensitive adhesive sheet, comprising the steps of forming a coating layer of a pressure-sensitive adhesive-containing composition on a substrate, arranging a liner on the surface of the coating layer to form a laminate, and a humidification and heating step of placing the laminate in a temperature- and humidity-controlled environment for a predetermined humidification and heating time (e.g., 2 hours to 7 days), wherein the product of the humidification and heating time, temperature, and humidity in the humidification and heating step is 100 to 300,000°C·RH%·h. Effect of the Invention

[0007] According to the present invention, it is possible to provide a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer on the surface of which a sealing resin for sealing a semiconductor chip or the like can flow with little variation. [Brief description of the drawings]

[0008] [Figure 1] 1 is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to another embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic cross-sectional view of a liner-attached double-sided PSA sheet according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] A. Overview of adhesive sheets 1 is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention. The pressure-sensitive adhesive sheet 100 comprises a substrate 10 and a pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer) 20 disposed on at least one side of the substrate 10.

[0010] The adhesive sheet of the present invention has an adhesive strength of 0.1 N / 20 mm to 8 N / 20 mm at 23° C. when the adhesive layer is attached to polyethylene terephthalate. The adhesive layer is made of an adhesive containing a base polymer, and the sp value of the base polymer is 7 (cal / cm 3 ) 1 / 2 ~10(cal / cm 3 ) 1 / 2 The pressure-sensitive adhesive sheet has a moisture content of 0.05% to 6% by weight.

[0011] The pressure-sensitive adhesive sheet of the present invention can be suitably used as a temporary fixing material when a semiconductor chip is resin-sealed. More specifically, the pressure-sensitive adhesive sheet of the present invention can be used as a temporary fixing material for a semiconductor chip when the semiconductor chip is arranged on the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet, the semiconductor chip is covered with a precursor of a sealing resin (usually an epoxy resin), and the sealing resin precursor is cured to resin-seal the semiconductor chip. After the semiconductor chip is resin-sealed, the pressure-sensitive adhesive sheet can be peeled off from the structure composed of the sealing resin and the semiconductor chip during a predetermined post-process (for example, back grinding of the sealing resin, pattern formation, bump formation, chipping (cutting)). The epoxy equivalent of the sealing resin is, for example, 50 g / eq to 500 g / eq.

[0012] In the pressure-sensitive adhesive sheet of the present invention, as described above, the sp value of the base polymer contained in the pressure-sensitive adhesive layer is specified, and the moisture content of the pressure-sensitive adhesive sheet is specified, so that the encapsulating resin precursor can flow favorably on the pressure-sensitive adhesive layer. In addition, since the variation in the flowability of the encapsulating resin precursor is suppressed, the time of the encapsulation process can be shortened in the mass production process of semiconductor chips, and resin encapsulation with excellent uniformity can be stably performed. In this way, the pressure-sensitive adhesive sheet of the present invention is characterized by having an excellent balance between adhesion and peelability (i.e., excellent temporary fixation), and being able to contribute to improving encapsulation quality. In addition, the pressure-sensitive adhesive sheet of the present invention is particularly useful in that it can contribute to improving encapsulation quality even at high temperatures.

[0013] 2 is a schematic cross-sectional view of a pressure-sensitive adhesive sheet according to another embodiment of the present invention. The pressure-sensitive adhesive sheet 200 is a double-sided pressure-sensitive adhesive sheet, and further comprises a second pressure-sensitive adhesive layer 30 on the side of the substrate 10 opposite the pressure-sensitive adhesive layer 20. That is, the pressure-sensitive adhesive sheet 200 comprises the pressure-sensitive adhesive layer 20, the substrate 10, and the second pressure-sensitive adhesive layer 30, in this order. By providing the second pressure-sensitive adhesive layer 30, when performing resin sealing on a base, the second pressure-sensitive adhesive layer 30 side can be attached to the base, and the pressure-sensitive adhesive sheet 200 can be used with good fixation.

[0014] In one embodiment, the second pressure-sensitive adhesive layer contains heat-expandable microspheres. The heat-expandable microspheres can expand at a predetermined temperature. When the pressure-sensitive adhesive layer containing such heat-expandable microspheres is heated to a predetermined temperature or higher, the heat-expandable microspheres expand, causing unevenness on the adhesive surface (i.e., the surface of the second pressure-sensitive adhesive layer), and the adhesive strength is reduced or lost. If a second pressure-sensitive adhesive layer containing heat-expandable microspheres is formed, the necessary adhesiveness is exhibited when the pressure-sensitive adhesive sheet is fixed (e.g., when fixed to a base), and when the pressure-sensitive adhesive sheet is peeled off (e.g., when peeled off from the base), the adhesive strength is reduced or lost by heating, and good peelability is exhibited.

[0015] The adhesive strength of the adhesive sheet of the present invention at 23°C when the adhesive layer is attached to polyethylene terephthalate is, as described above, 0.1N / 20mm to 8N / 20mm, preferably 0.2N / 20mm to 7.5N / 20mm, more preferably 0.5N / 20mm to 6N / 20mm, even more preferably 0.8N / 20mm to 5N / 20mm, and most preferably 0.8N / 20mm to 3N / 20mm. If it is within such a range, it is possible to obtain an adhesive sheet that can favorably fix an adherend (e.g., a semiconductor chip) and leaves little adhesive residue when peeled off. In this specification, "adhesive strength at 23°C when the adhesive layer is attached to polyethylene terephthalate" refers to the adhesive strength measured by laminating the adhesive layer of an adhesive sheet (width 20 mm × length 140 mm) to a polyethylene terephthalate film (thickness 25 μm) (lamination conditions: one round trip with a 2 kg roller), leaving the sample at an environmental temperature of 23°C for 30 minutes, and then subjecting the sample to a tensile test (peel speed: 300 mm / min, peel angle 180°).

[0016] As described above, the moisture content of the pressure-sensitive adhesive sheet is 0.05% by weight to 6% by weight. The moisture content of the pressure-sensitive adhesive sheet is preferably 0.1% by weight to 5% by weight, more preferably 0.5% by weight to 4% by weight, and even more preferably 1% by weight to 3% by weight. Within such a range, the affinity with the encapsulating resin precursor can be appropriately adjusted, and a pressure-sensitive adhesive layer that can contribute to improving the resin encapsulation quality can be formed. In addition, deterioration of the encapsulating resin can be prevented. The moisture content can be measured by Karl Fischer titration. The moisture content of the pressure-sensitive adhesive sheet can be adjusted by any appropriate method. For example, it can be adjusted by adjusting the moisture content of the pressure-sensitive adhesive when forming the pressure-sensitive adhesive layer (when applying the pressure-sensitive adhesive), the composition of the base polymer contained in the pressure-sensitive adhesive, carrying out a humidification and heating process (described later), and the like.

[0017] The thickness of the pressure-sensitive adhesive sheet of the present invention is preferably 3 μm to 300 μm, more preferably 5 μm to 150 μm, and even more preferably 10 μm to 100 μm.

[0018] B.Adhesive layer The pressure-sensitive adhesive layer is composed of a pressure-sensitive adhesive containing a base polymer. The term "base polymer" refers to the main component of the polymer contained in the pressure-sensitive adhesive. In this specification, the term "main component" refers to a component contained in an amount of more than 50% by weight, unless otherwise specified.

[0019] The thickness of the pressure-sensitive adhesive layer is preferably 1 μm to 50 μm, more preferably 3 μm to 30 μm, and even more preferably 5 μm to 20 μm. Within this range, it is possible to obtain a pressure-sensitive adhesive sheet that is unlikely to cause the semiconductor chip to become embedded in the resin even when pressure is applied during the encapsulation step. In one embodiment, the thickness of the pressure-sensitive adhesive layer is 2 μm to 15 μm. Within this range, the dissipation of moisture from the pressure-sensitive adhesive layer can be appropriately controlled, and the fluidity of the encapsulation resin precursor can be made favorable.

[0020] As mentioned above, the sp value of the base polymer is 7 (cal / cm 3 ) 1 / 2 ~10(cal / cm 3 ) 1 / 2 The sp value of the base polymer is preferably 7.5 (cal / cm 3 ) 1 / 2 ~9.5(cal / cm 3 ) 1 / 2 and more preferably 8 (cal / cm 3 ) 1 / 2 ~9(cal / cm 3 ) 1 / 2Within this range, the affinity for the sealing resin is appropriately adjusted, and a pressure-sensitive adhesive layer that can contribute to improving the quality of resin sealing can be formed. The sp value is determined by the Fedors method (Hideki Yamamoto, "sp Value Basics, Applications and Calculation Methods", Johokki Publishing Co., Ltd., published on April 3, 2006, pages 66-67). Specifically, the sp value is calculated from the evaporation energy Δe (cal) at 25°C of each atom or atomic group forming the polymer and the molar volume ΔV (cm3) at 25°C of each atom or atomic group forming the polymer according to the following formula. When the polymer is a copolymer, the sp value is calculated by calculating the sp value of each homopolymer of each constituent unit constituting the copolymer, and adding up the values ​​obtained by multiplying each of these sp values ​​by the molar fraction of each constituent unit. sp value = (ΣΔe / ΣΔv) 1 / 2

[0021] The water contact angle of the pressure-sensitive adhesive layer is preferably 70° to 120°, more preferably 80° to 110°, and even more preferably 90° to 105°. Within such a range, the affinity with the encapsulating resin precursor can be appropriately adjusted, and a pressure-sensitive adhesive layer that can contribute to improving the resin encapsulation quality can be formed. The water contact angle can be determined by using a contact angle meter (for example, Kyowa Interface Co., Ltd., product name "CX-A type") to drop 2 μl of pure water onto the surface of the pressure-sensitive adhesive layer in a 23° C. / 50% RH environment, and measuring the contact angle of the droplet 5 seconds after dropping, repeating this process five times, and then calculating the average value.

[0022] The gel fraction of the pressure-sensitive adhesive layer is preferably 60% to 100%, more preferably 70% to 99%, even more preferably 75% to 98%, and particularly preferably 80% to 95%. Within such a range, the dissipation of moisture from the pressure-sensitive adhesive layer can be appropriately controlled, and the fluidity of the encapsulating resin precursor can be made favorable. In addition, a pressure-sensitive adhesive layer can be formed that has appropriate adhesion, does not leave adhesive residue when peeled off, and does not easily contaminate the adherend. The method for measuring the gel fraction will be described later.

[0023] The elastic modulus of the pressure-sensitive adhesive layer at 25°C measured by nanoindentation is preferably less than 100 MPa, more preferably 0.1 MPa to 50 MPa, and even more preferably 0.1 MPa to 10 MPa. Within such a range, an adhesive sheet having an appropriate adhesive strength can be obtained. The elastic modulus measured by nanoindentation refers to an elastic modulus obtained by continuously measuring the load applied to the indenter and the indentation depth during loading and unloading when the indenter is pressed into the sample, and then obtaining a load-indentation depth curve. In this specification, the elastic modulus measured by nanoindentation refers to an elastic modulus measured as described above under the measurement conditions of load: 1 mN, loading / unloading rate: 0.1 mN / s, and holding time: 1 s.

[0024] (Acrylic adhesive) In one embodiment, the adhesive constituting the adhesive layer is an acrylic adhesive. Examples of the acrylic adhesive include an acrylic polymer (homopolymer or copolymer) using one or more (meth)acrylic acid alkyl esters as a monomer component as a prepolymer, and an acrylic adhesive having a crosslinked body of the prepolymer as a base polymer. In this specification, the "base polymer" contained in the acrylic adhesive in the adhesive layer means a polymer formed by crosslinking a prepolymer (uncrosslinked polymer). In one embodiment, the base polymer has a crosslinked body structure of an acrylic polymer and an epoxy crosslinking agent.

[0025] Specific examples of the (meth)acrylic acid alkyl ester include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, and ) acrylate nonyl, (meth)acrylate isononyl, (meth)acrylate decyl, (meth)acrylate isodecyl, (meth)acrylate undecyl, (meth)acrylate dodecyl, (meth)acrylate tridecyl, (meth)acrylate tetradecyl, (meth)acrylate pentadecyl, (meth)acrylate hexadecyl, (meth)acrylate heptadecyl, (meth)acrylate octadecyl, (meth)acrylate nonadecyl, (meth)acrylate eicosyl, etc. (meth)acrylic acid C1-20 alkyl esters are included. Among them, (meth)acrylic acid alkyl esters having a linear or branched alkyl group having 4 to 20 carbon atoms (more preferably 6 to 20, particularly preferably 8 to 18) are preferred, and (meth)acrylate 2-ethylhexyl is more preferred. In this specification, (meth)acrylic means acrylic and / or methacrylic.

[0026] The acrylic polymer (prepolymer) may contain units corresponding to other monomer components copolymerizable with the (meth)acrylic acid alkyl ester, if necessary, for the purpose of modifying the cohesive strength, heat resistance, crosslinkability, etc. Examples of such monomer components include carboxyl group-containing monomers such as acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, and crotonic acid; acid anhydride monomers such as maleic anhydride and itanoic anhydride; hydroxyl group-containing monomers such as hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, hydroxyhexyl (meth)acrylate, hydroxyoctyl (meth)acrylate, hydroxydecyl (meth)acrylate, hydroxylauryl (meth)acrylate, and (4-hydroxymethylcyclohexyl)methyl methacrylate; sulfonic acid group-containing monomers such as styrene sulfonic acid, allyl sulfonic acid, 2-(meth)acrylamido-2-methylpropanesulfonic acid, (meth)acrylamidopropanesulfonic acid, sulfopropyl (meth)acrylate, and (meth)acryloyloxynaphthalenesulfonic acid; (N-substituted) amide monomers such as N,N-dimethyl(meth)acrylamide, N-butyl(meth)acrylamide, N-methylol(meth)acrylamide, and N-methylolpropane(meth)acrylamide; aminoalkyl(meth)acrylate monomers such as aminoethyl(meth)acrylate, N,N-dimethylaminoethyl(meth)acrylate, and t-butylaminoethyl(meth)acrylate; alkoxyalkyl(meth)acrylate monomers such as methoxyethyl(meth)acrylate and ethoxyethyl(meth)acrylate; maleimide monomers such as N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, and N-phenylmaleimide; itaconimide monomers such as N-methylitaconimide, N-ethylitaconimide, N-butylitaconimide, N-octylitaconimide, N-2-ethylhexylitaconimide, N-cyclohexylitaconimide, and N-laurylitaconimide;succinimide monomers such as N-(meth)acryloyloxymethylene succinimide, N-(meth)acryloyl-6-oxyhexamethylene succinimide, and N-(meth)acryloyl-8-oxyoctamethylene succinimide; vinyl monomers such as vinyl acetate, vinyl propionate, N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, N-vinyl carboxylic acid amides, styrene, α-methylstyrene, and N-vinylcaprolactam; cyanoacrylate monomers such as acrylonitrile and methacrylonitrile; epoxy group-containing acrylic monomers such as glycidyl (meth)acrylate; polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and (meth)acrylate. Examples of the monomers include glycol-based acrylic ester monomers such as methoxy polypropylene glycol (meth)acrylate; acrylic ester monomers having heterocycles, halogen atoms, silicon atoms, etc., such as tetrahydrofurfuryl (meth)acrylate, fluorine (meth)acrylate, and silicone (meth)acrylate; polyfunctional monomers such as hexanediol di(meth)acrylate, (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, epoxy acrylate, polyester acrylate, and urethane acrylate; olefin-based monomers such as isoprene, butadiene, and isobutylene; and vinyl ether-based monomers such as vinyl ether. These monomer components may be used alone or in combination of two or more.

[0027] In one embodiment, the acrylic polymer (prepolymer) further contains a constituent unit derived from a hydroxyl group-containing monomer. The content of the constituent unit derived from a hydroxyl group-containing monomer is preferably 0.1 to 20 parts by weight, more preferably 0.1 to 10 parts by weight, relative to 100 parts by weight of all constituent units constituting the acrylic polymer. More preferably, it is 0.5 to 10 parts by weight. Within such a range, the dissipation of moisture from the pressure-sensitive adhesive layer is appropriately controlled, and a pressure-sensitive adhesive layer with a preferably adjusted moisture content can be formed. In addition, a pressure-sensitive adhesive layer having appropriate cohesiveness and little adhesive residue can be formed. The hydroxyl group may be an alcoholic hydroxyl group or an acidic hydroxyl group such as a carboxyl group.

[0028] The acrylic adhesive may contain any suitable additives as necessary, such as crosslinkers, tackifiers, plasticizers (e.g., trimellitic acid ester plasticizers, pyromellitic acid ester plasticizers, etc.), pigments, dyes, fillers, antioxidants, conductive materials, antistatic agents, UV absorbers, light stabilizers, release regulators, softeners, surfactants, flame retardants, antioxidants, etc.

[0029] Examples of the crosslinking agent contained in the acrylic adhesive include an isocyanate-based crosslinking agent, an epoxy-based crosslinking agent, a melamine-based crosslinking agent, a peroxide-based crosslinking agent, as well as a urea-based crosslinking agent, a metal alkoxide-based crosslinking agent, a metal chelate-based crosslinking agent, a metal salt-based crosslinking agent, a carbodiimide-based crosslinking agent, an oxazoline-based crosslinking agent, an aziridine-based crosslinking agent, and an amine-based crosslinking agent.

[0030] In one embodiment, the amount of the crosslinking agent relative to the carboxyl group of the acrylic polymer (prepolymer) is preferably 0.08 to 2 molar equivalents, more preferably 0.1 to 1 molar equivalent. Within such a range, an acrylic pressure-sensitive adhesive having a high crosslinking density can be formed, and component migration between the pressure-sensitive adhesive layer and the sealing resin is preferably prevented. The amount of the crosslinking agent used here means the content of the crosslinking agent before the acrylic polymer is crosslinked.

[0031] Specific examples of the isocyanate-based crosslinking agent contained in the acrylic pressure-sensitive adhesive include lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate; alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate; aromatic isocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate and xylylene diisocyanate; and isocyanate adducts such as trimethylolpropane / tolylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate L"), trimethylolpropane / hexamethylene diisocyanate trimer adduct (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate HL"), and isocyanurate of hexamethylene diisocyanate (manufactured by Nippon Polyurethane Industry Co., Ltd., product name "Coronate HX"). The amount of the isocyanate crosslinking agent can be set to any appropriate amount depending on the desired adhesive strength, and is typically 0.1 to 20 parts by weight, more preferably 1 to 10 parts by weight, relative to 100 parts by weight of the acrylic polymer. Within this range, a pressure-sensitive adhesive sheet with fewer residual carboxyl groups in the components in the pressure-sensitive adhesive layer can be obtained. The amount of the crosslinking agent used here means the content of the crosslinking agent before the acrylic polymer is crosslinked.

[0032] Examples of the epoxy crosslinking agent contained in the acrylic adhesive include N,N,N',N'-tetraglycidyl-m-xylylenediamine, diglycidylaniline, 1,3-bis(N,N-glycidylaminomethyl)cyclohexane (manufactured by Mitsubishi Gas Chemical Company, Inc., product name "Tetrad C"), 1,6-hexanediol diglycidyl ether (manufactured by Kyoeisha Chemical Company, Inc., product name "Epolite 1600"), neopentyl glycol diglycidyl ether (manufactured by Kyoeisha Chemical Company, Inc., product name "Epolite 1500NP"), ), ethylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., product name "Epolight 40E"), propylene glycol diglycidyl ether (manufactured by Kyoeisha Chemical Co., Ltd., product name "Epolight 70P"), polyethylene glycol diglycidyl ether (manufactured by Nippon Oil & Fats Co., Ltd., product name "Epiol E-400"), polypropylene glycol diglycidyl ether (manufactured by Nippon Oil & Fats Co., Ltd., product name "Epiol P-200"), sorbitol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, product name "Denacol" Examples of the epoxy resins include glycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-611"), glycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-314"), pentaerythritol polyglycidyl ether, polyglycerol polyglycidyl ether (manufactured by Nagase ChemteX Corporation, trade name "Denacol EX-512"), sorbitan polyglycidyl ether, trimethylolpropane polyglycidyl ether, adipic acid diglycidyl ester, o-phthalic acid diglycidyl ester, triglycidyl-tris(2-hydroxyethyl)isocyanurate, resorcinol diglycidyl ether, bisphenol-S-diglycidyl ether, and epoxy resins having two or more epoxy groups in the molecule. The amount of the epoxy crosslinking agent may be set to any appropriate amount depending on the desired adhesive strength, and is typically 0.01 to 50 parts by weight, more preferably 0.6 to 15 parts by weight, even more preferably 2 to 13 parts by weight, and particularly preferably 3 to 10 parts by weight, relative to 100 parts by weight of the acrylic polymer. If the amount is within such a range, a pressure-sensitive adhesive sheet having a small amount of residual carboxyl groups in the components in the pressure-sensitive adhesive layer can be obtained. The amount of the crosslinking agent used here means the content of the crosslinking agent before the acrylic polymer is crosslinked.

[0033] C. Base material Examples of the substrate include resin sheets, nonwoven fabrics, paper, metal foils, woven fabrics, rubber sheets, foam sheets, and laminates thereof (particularly laminates containing resin sheets). Examples of the resins constituting the resin sheets include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polyethylene (PE), polypropylene (PP), ethylene-propylene copolymers, ethylene-vinyl acetate copolymers (EVA), polyamides (nylons), wholly aromatic polyamides (aramids), polyimides (PI), polyvinyl chloride (PVC), polyphenylene sulfide (PPS), fluorine-based resins, and polyether ether ketones (PEEK). Examples of the nonwoven fabrics include nonwoven fabrics made of natural fibers having heat resistance, such as nonwoven fabrics containing Manila hemp; synthetic resin nonwoven fabrics such as polypropylene resin nonwoven fabrics, polyethylene resin nonwoven fabrics, and ester resin nonwoven fabrics. Examples of the metal foils include copper foils, stainless steel foils, and aluminum foils. Examples of the paper include Japanese paper and craft paper.

[0034] In one embodiment, a resin sheet made of a resin having a glass transition temperature (Tg) of 60°C to 450°C (preferably 65°C to 430°C, more preferably 80°C to 420°C) is preferably used as the substrate. By using such a resin sheet, even during heating (for example, heating during a sealing process), the molecular motion of the molecules constituting the substrate does not become too intense, and the dissipation of moisture can be appropriately suppressed. In addition, a pressure-sensitive adhesive sheet with excellent flexibility can be obtained. Examples of resins constituting such a resin sheet include polyethylene terephthalate, polyimide, and polyethylene naphthalate.

[0035] In one embodiment, the substrate is made of an aromatic polyimide resin. Aromatic polyimide resins are preferred because the imide group is a polar functional group, and because the electron donating property of the amino group and the electron withdrawing property of the carbonyl group make it easy to adjust the moisture content, and because the resin sealing process requires a wide range of high processing temperatures, and the resin sealing process requires a wide range of high processing temperatures. In addition, aromatic functional groups (phenyl, phenylene, naphthyl, naphthylene, etc.) are contained in large amounts, so the molecular mobility of the polymer molecules is low, and the tape surface shape is kept smooth. This makes it easy for resin flow to occur uniformly, and is therefore very favorable for solving the problems of the present invention. Examples of aromatic polyimides include ether-based polyphthalimides having an ether bond in the main chain skeleton, ketone-based polyphthalimides having a ketone bond, and bisphenol-based polyphthalimides having a skeleton derived from the bisphenol. Commercially available products such as "UPILEX" manufactured by Ube Industries, Ltd., "LARC-TPI" manufactured by Mitsui Chemicals, Inc., and "Ultem" manufactured by GE may also be used. In particular, ether-based pyromellitimides having an ether bond in the main chain skeleton are preferably used because they have a large number of imide groups per unit weight of the repeating monomer residue. Commercially available resins such as "Kapton" manufactured by DuPont, "Apical" manufactured by Kaneka, and "Aurum" manufactured by Mitsui Chemicals, Inc. may be used.

[0036] The thickness of the substrate can be set to any appropriate thickness depending on the desired strength or flexibility, the purpose of use, etc. The thickness of the substrate is preferably 1000 μm or less, more preferably 25 μm to 1000 μm, and further preferably 40 μm to 500 μm.

[0037] The substrate may be subjected to a surface treatment, such as corona treatment, chromate treatment, ozone exposure, flame exposure, high-voltage shock exposure, ionizing radiation treatment, or coating with a primer.

[0038] Examples of the organic coating material include materials described in Plastic Hard Coat Materials II (CMC Publishing, (2004)). Preferably, a urethane-based polymer is used, more preferably polyacrylic urethane, polyester urethane, or a precursor thereof. This is because coating and application to a substrate is simple, and a wide variety of materials can be selected industrially and are inexpensively available. The urethane-based polymer is, for example, a polymer made of a reaction mixture of an isocyanate monomer and an alcoholic hydroxyl group-containing monomer (for example, a hydroxyl group-containing acrylic compound or a hydroxyl group-containing ester compound). The organic coating material may contain, as an optional additive, a chain extender such as polyamine, an antiaging agent, an oxidation stabilizer, and the like. The thickness of the organic coating layer is not particularly limited, but is, for example, suitable to be about 0.1 μm to 10 μm, preferably about 0.1 μm to 5 μm, and more preferably about 0.5 μm to 5 μm.

[0039] D. Second Adhesive Layer The second pressure-sensitive adhesive layer may be a pressure-sensitive adhesive layer composed of any appropriate pressure-sensitive adhesive. In one embodiment, as described above, the second pressure-sensitive adhesive layer further contains heat-expandable microspheres.

[0040] The adhesive contained in the second adhesive layer may be a curable adhesive (for example, an active energy ray curable adhesive) or a pressure-sensitive adhesive. Examples of pressure-sensitive adhesives include acrylic adhesives and rubber-based adhesives. For details of the adhesive contained in the second adhesive layer, reference may be made to the description in, for example, JP 2018-009050 A. The entire description of this publication is incorporated herein by reference. In one embodiment, the adhesive contained in the second adhesive layer may be the acrylic adhesive described in the above section B. In one embodiment, as described in the above section B, the acrylic polymer (prepolymer) contained in the acrylic adhesive contains a constituent unit derived from a hydroxyl group-containing monomer. The content of the constituent unit derived from the hydroxyl group-containing monomer is preferably 0.1 to 20 parts by weight, more preferably 0.1 to 10 parts by weight, relative to 100 parts by weight of all constituent units constituting the acrylic polymer. More preferably, it is 0.5 to 10 parts by weight.

[0041] As the heat-expandable microspheres, any suitable heat-expandable microspheres can be used so long as they are microspheres that can expand or foam when heated. For example, the heat-expandable microspheres can be microspheres in which a substance that easily expands when heated (a volatile substance such as an organic solvent) is encapsulated in an elastic shell. Such heat-expandable microspheres can be produced by any suitable method, such as a coacervation method or an interfacial polymerization method.

[0042] Examples of substances that easily expand when heated include low-boiling liquids such as propane, propylene, butene, normal butane, isobutane, isopentane, neopentane, normal pentane, normal hexane, isohexane, heptane, octane, petroleum ether, methane halides, and tetraalkylsilanes; azodicarbonamide that gasifies by thermal decomposition; and the like.

[0043] Examples of materials constituting the shell include polymers composed of nitrile monomers such as acrylonitrile, methacrylonitrile, α-chloroacrylonitrile, α-ethoxyacrylonitrile, and fumaronitrile; carboxylic acid monomers such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, fumaric acid, and citraconic acid; vinylidene chloride; vinyl acetate; (meth)acrylic acid esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, benzyl (meth)acrylate, and β-carboxyethyl acrylate; styrene monomers such as styrene, α-methylstyrene, and chlorostyrene; and amide monomers such as acrylamide, substituted acrylamide, methacrylamide, and substituted methacrylamide. Polymers composed of these monomers may be homopolymers or copolymers. Examples of such copolymers include vinylidene chloride-methyl methacrylate-acrylonitrile copolymer, methyl methacrylate-acrylonitrile-methacrylonitrile copolymer, methyl methacrylate-acrylonitrile copolymer, acrylonitrile-methacrylonitrile-itaconic acid copolymer, and the like.

[0044] In the polymer constituting the shell, the constituent unit derived from the carboxyl group-containing monomer is preferably 80 parts by weight or less, more preferably 70 parts by weight or less, based on 100 parts by weight of the polymer constituting the shell. Within such a range, a second pressure-sensitive adhesive layer having an appropriately adjusted water content can be formed.

[0045] Details of the "substance that expands easily upon heating" and the "shell" that constitute the heat-expandable microspheres are also described in, for example, JP 2018-141086 A. This document is incorporated herein by reference.

[0046] The heat-expandable microspheres may be made of an inorganic or organic foaming agent, such as ammonium carbonate, ammonium hydrogen carbonate, sodium hydrogen carbonate, ammonium nitrite, sodium borohydride, and various azides. Examples of organic foaming agents include fluorinated alkane compounds such as trichloromonofluoromethane and dichloromonofluoromethane; azo compounds such as azobisisobutyronitrile, azodicarbonamide and barium azodicarboxylate; hydrazine compounds such as paratoluenesulfonylhydrazide, diphenylsulfone-3,3'-disulfonylhydrazide, 4,4'-oxybis(benzenesulfonylhydrazide) and allylbis(sulfonylhydrazide); semicarbazide compounds such as p-toluylenesulfonylsemicarbazide and 4,4'-oxybis(benzenesulfonylsemicarbazide); triazole compounds such as 5-morpholyl-1,2,3,4-thiatriazole; and N-nitroso compounds such as N,N'-dinitrosopentamethylenetetramine and N,N'-dimethyl-N,N'-dinitrosoterephthalamide.

[0047] The heat-expandable microspheres may be commercially available products. Specific examples of commercially available heat-expandable microspheres include "Matsumoto Microsphere" (product name: F-30, F-30D, F-36D, F-36LV, F-50, F-50D, F-65, F-65D, FN-100SS, FN-100SSD, FN-180SS, FN-180SSD, F-190D, F-260D, F-2800D) manufactured by Matsumoto Yushi Seiyaku Co., Ltd., and "Expancel" (product name: 053 -40, 031-40, 920-40, 909-80, 930-120), "Dieform" manufactured by Kureha Chemical Industry Co., Ltd. (grades: H750, H850, H1100, S2320D, S2640D, M330, M430, M520), and "Advancell" manufactured by Sekisui Chemical Co., Ltd. (grades: EML101, EMH204, EHM301, EHM302, EHM303, EM304, EHM401, EM403, EM501).

[0048] The average particle size (by number) of the heat-expandable microspheres before heating is preferably 1 to 40 μm, more preferably 5 to 40 μm, and further preferably 10 to 40 μm. The particle size and average particle size are values ​​determined by a particle size distribution measurement method using a laser scattering method.

[0049] The heat-expandable microspheres preferably have an appropriate strength so that they do not burst until their volumetric expansion rate reaches at least 5 times, more preferably at least 7 times, and even more preferably at least 10 times. When such heat-expandable microspheres are used, their adhesive strength can be efficiently reduced by heat treatment.

[0050] The content of the heat-expandable microspheres in the second pressure-sensitive adhesive layer can be appropriately set depending on the desired decrease in adhesive strength, etc. The content of the heat-expandable microspheres is, for example, 1 to 150 parts by weight, preferably 10 to 130 parts by weight, and more preferably 25 to 100 parts by weight, relative to 100 parts by weight of the base polymer forming the second pressure-sensitive adhesive layer.

[0051] The arithmetic surface roughness Ra of the second pressure-sensitive adhesive layer before the expansion of the heat-expandable microspheres (i.e., before heating) is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less. Within such ranges, a pressure-sensitive adhesive sheet with excellent adhesion to an adherend can be obtained.

[0052] (Undercoat layer) When the pressure-sensitive adhesive sheet includes a second pressure-sensitive adhesive layer, an undercoat layer may be provided between the substrate and the second pressure-sensitive adhesive layer. The undercoat layer includes any appropriate pressure-sensitive adhesive. Examples of pressure-sensitive adhesives constituting the undercoat layer include acrylic pressure-sensitive adhesives, rubber pressure-sensitive adhesives, silicone pressure-sensitive adhesives, and the like. Among them, acrylic pressure-sensitive adhesives may be preferably used. In addition, an active energy ray-curable acrylic pressure-sensitive adhesive (hereinafter, active energy ray-curable pressure-sensitive adhesive) may be used as the pressure-sensitive adhesive. Preferably, the same pressure-sensitive adhesive as the pressure-sensitive adhesive constituting the second pressure-sensitive adhesive layer is used as the pressure-sensitive adhesive constituting the undercoat layer.

[0053] The thickness of the undercoat layer is preferably from 1 μm to 40 μm, more preferably from 5 μm to 35 μm, and further preferably from 10 μm to 30 μm.

[0054] E. Manufacturing method of adhesive sheet The pressure-sensitive adhesive sheet of the present invention can be produced by any suitable method. For example, the method of obtaining the pressure-sensitive adhesive sheet of the present invention includes a method of directly coating a composition containing a pressure-sensitive adhesive (e.g., an acrylic pressure-sensitive adhesive) on a substrate, or a method of coating a composition containing a pressure-sensitive adhesive on any suitable substrate and transferring the formed coating layer to the substrate. The composition containing an acrylic pressure-sensitive adhesive can contain any suitable solvent.

[0055] The composition containing the pressure-sensitive adhesive contains any appropriate solvent, the moisture content of which is preferably 0.003% by weight to 0.3% by weight.

[0056] When forming a pressure-sensitive adhesive layer containing heat-expandable microspheres (second pressure-sensitive adhesive layer), the pressure-sensitive adhesive layer can be formed by coating a substrate with a composition containing heat-expandable microspheres, a pressure-sensitive adhesive, and any suitable solvent. Alternatively, the pressure-sensitive adhesive layer containing heat-expandable microspheres may be formed by sprinkling heat-expandable microspheres on the pressure-sensitive adhesive coating layer and then embedding the heat-expandable microspheres in the pressure-sensitive adhesive using a laminator or the like.

[0057] Any suitable coating method can be adopted as the coating method of the pressure sensitive adhesive and each composition. For example, each layer can be formed by drying after coating. For example, coating methods include coating methods using a multi-coater, a die coater, a gravure coater, an applicator, etc. For example, drying methods include natural drying, heat drying, etc. When heat drying is performed, the heating temperature can be set to any suitable temperature according to the characteristics of the material to be dried.

[0058] In one embodiment, a coating layer of a composition containing a pressure-sensitive adhesive is formed on a substrate, and then a liner is placed on the coating layer surface to obtain a laminate (a pressure-sensitive adhesive sheet precursor with a liner). The laminate (a pressure-sensitive adhesive sheet precursor with a liner) is placed in a temperature- and humidity-controlled environment for a predetermined humidification and heating time (for example, 2 hours to 7 days) (humidification and heating step) to obtain a pressure-sensitive adhesive sheet. By carrying out the humidification and heating step, the moisture content of the pressure-sensitive adhesive sheet can be preferably adjusted. The temperature in this step is, for example, 40°C to 120°C. The humidity is, for example, 1% RH to 100% RH. When the pressure-sensitive adhesive sheet is a double-sided pressure-sensitive adhesive sheet, a laminate obtained by placing liners (a first liner and a second liner) on both sides of the coating layer surface of the pressure-sensitive adhesive (i.e., the coating layer surface of the pressure-sensitive adhesive that forms the pressure-sensitive adhesive layer and the coating layer surface of the pressure-sensitive adhesive that forms the second pressure-sensitive adhesive layer) can be subjected to the humidification and heating step. Details of the liners will be described later.

[0059] In the humidification and heating step, the product of the humidification and heating time, temperature and humidity is preferably 100 to 300,000° C.·RH%·h, and more preferably 180 to 265,000° C.·RH%·h. Within this range, the moisture content of the pressure-sensitive adhesive sheet can be preferably adjusted.

[0060] F. Double-sided adhesive sheet with liner FIG. 3 is a schematic cross-sectional view of a liner-attached double-sided adhesive sheet according to one embodiment of the present invention. The liner-attached double-sided adhesive sheet 110 comprises a double-sided adhesive sheet 200, a first liner 40 disposed directly on one side of the adhesive sheet 200 in a releasable manner, and a second liner 50 disposed directly on the other side of the double-sided adhesive sheet 200 in a releasable manner. By disposing the first liner 40 and the second liner 50, it is possible to protect the adhesive layer from contamination and prevent blocking of the roll-shaped or sheet-shaped double-sided adhesive sheet. Typically, the first liner and the second liner comprise a liner substrate and a release treatment layer disposed on at least one side of the liner substrate. The first liner and the second liner are disposed so that the release treatment layer faces the double-sided adhesive sheet.

[0061] The double-sided pressure-sensitive adhesive sheet 200 may be the pressure-sensitive adhesive sheet described above, that is, a pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer 20, a substrate 10, and a second pressure-sensitive adhesive layer 30.

[0062] The first liner 20 and the second liner 30 may be of different nature. Being "of different nature" may mean, for example, that they have different thicknesses (for example, the absolute value of the difference in thickness is 1 μm or more (preferably 5 μm or more, more preferably 10 μm or more)), that they have different colors, that they are made of different materials, etc. The difference in thickness between the first liner 20 and the second liner 30 is preferably 70 μm or less, more preferably 50 μm or less, and even more preferably 25 μm or less.

[0063] In one embodiment, when the liner-attached double-sided pressure-sensitive adhesive sheet is used, the first liner is peeled off first. More specifically, the liner-attached double-sided pressure-sensitive adhesive sheet can be used by first peeling off the first liner, attaching an adherend (e.g., electronic components) to the exposed adhesive surface (e.g., the surface of the first pressure-sensitive adhesive layer), and then peeling off the second liner, and attaching the surface of the second pressure-sensitive adhesive layer to another adherend (e.g., a base). In such an embodiment, the adherend (e.g., electronic components) is temporarily fixed to the base via the pressure-sensitive adhesive sheet; the adherend is subjected to a predetermined processing; and then the adhesive strength of the second pressure-sensitive adhesive layer is reduced by heating, and the pressure-sensitive adhesive sheet with the adherend is peeled off from the base. As described above, if the first liner and the second liner are different in nature, it becomes easy to identify the liner to be peeled off at a predetermined timing.

[0064] The peel strength of the first liner from the double-sided adhesive sheet is preferably 0.001 N / 50 mm to 2 N / 50 mm, more preferably 0.01 N / 50 mm to 1.5 N / 50 mm, even more preferably 0.05 N / 50 mm to 1 N / 50 mm, and particularly preferably 0.1 N / 50 mm to 0.8 N / 50 mm. The peel strength of the first liner from the double-sided adhesive sheet (and the peel strength of the second liner from the double-sided adhesive sheet) refers to the adhesive strength measured by peeling the liner from the double-sided adhesive sheet of the liner-attached double-sided adhesive sheet (peel angle: 180°, peel speed (tensile speed): 300 mm / min) in an environment of 23° C. The peel strength of the liner from the double-sided adhesive sheet can be adjusted by any appropriate method, such as the composition of the adhesive layer, the type of liner, or the surface treatment applied to the liner.

[0065] The peel strength of the second liner from the double-sided pressure-sensitive adhesive sheet is preferably 0.001 N / 50 mm to 2 N / 50 mm, more preferably 0.01 N / 50 mm to 1.5 N / 50 mm, even more preferably 0.05 N / 50 mm to 1 N / 50 mm, and particularly preferably 0.1 N / 50 mm to 0.8 N / 50 mm.

[0066] The thickness of the first liner is preferably 5 μm to 250 μm, more preferably 10 μm to 200 μm, even more preferably 20 to 150 μm, and most preferably 30 to 100 μm. The thickness of the second liner is preferably 5 μm to 250 μm, more preferably 10 μm to 200 μm, even more preferably 20 to 150 μm, and most preferably 30 to 100 μm.

[0067] The liner substrate may be made of any suitable material. The liner substrate may be, for example, a plastic film, a plastic sheet, or various sheet-like materials such as paper, cloth, nonwoven fabric, metal foil, or a plastic laminate thereof, or a laminate of plastics. Among them, plastic films and plastic sheets (hereinafter referred to as plastic films) are most preferable from the viewpoint of handling and cost. The material of the plastic film may be selected as necessary from the viewpoint of strength, heat resistance, etc. For example, olefin-based resins having α-olefin as a monomer component such as polyethylene (PE), polypropylene (PP), ethylene-propylene copolymer, and ethylene-vinyl acetate copolymer (EVA); polyesters such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); polyvinyl chloride (PVC); polyphenylene sulfide (PPS); amide-based resins such as polyamide (nylon) and fully aromatic polyamide (aramid); polyether ether ketone (PEEK), polyimide, polyetherimide, polystyrene, and acrylic resins may be mentioned. These materials can be used alone or in combination of two or more. The plastic film may be any of an unstretched film, a uniaxially oriented film, and a biaxially oriented film. These films may be laminated films consisting of two or more film layers, or from the viewpoint of handling, a film containing a lubricant such as inert particles may be appropriately added.

[0068] Any suitable treatment may be adopted as the treatment for forming the release treatment layer. In one embodiment, the release treatment layer is a silicone treatment layer. As the silicone, a reactive silicone compound whose main component is dimethylpolysiloxane and has a functional group required for crosslinking (curing) may be preferably used. This is because it can be applied to a film in a low molecular weight state, and can be cured after application to form a release treatment layer that is resistant to abrasion, etc. Examples of functional groups of reactive silicone compounds include vinyl groups, epoxy groups, alkoxy groups, and isocyanato groups.

[0069] The silicone-treated layer is formed, for example, by diluting the reactive silicone compound in a solvent or the like to adjust the concentration, and applying and heating the mixture using a gravure coater or the like. Heating promotes the drying of the solvent and the curing reaction. It is preferable to use a catalyst that promotes the curing reaction in combination. Examples of catalysts that can be used include complexes of metals such as platinum, palladium, rhodium, zirconium, and tin, organic bases such as amines, and organic acids such as acetic acid.

[0070] In one embodiment, the first liner and / or the second liner (substantially the release treatment layer of each liner) has an Si-Kα ray intensity by fluorescent X-ray analysis of 0.01 to 500 kcps (preferably 0.5 to 250 kcps, more preferably 1.0 to 150 kcps, even more preferably 1.05 to 100 kcps, and particularly preferably 10 to 30 kcps). Within such a range, the liner can be peeled off from the adhesive layer with a small force. In addition, the adhesion between the liner / adhesive layer becomes sufficient, and unnecessary peeling of the liner can be prevented. The Si-Kα ray intensity by fluorescent X-ray analysis is a value obtained by measuring the Si intensity of the release treatment agent layer and the non-release treatment agent layer by fluorescent X-ray analysis, respectively, and subtracting the strength of the non-release treatment agent layer from the strength of the release treatment agent layer. The strength can be adjusted by controlling the release treatment layer formation conditions, such as the application amount, concentration, application speed, and drying of the release treatment agent.

[0071] In one embodiment, the first liner and the second liner are different colors. A liner-attached double-sided pressure-sensitive adhesive sheet configured in this manner can be obtained, for example, by coloring one of the liners (for example, the liner substrate). If both liners are different colors, the front and back of the liner-attached double-sided pressure-sensitive adhesive sheet become clear, making it easy to identify the liner to be peeled off.

[0072] G.Applications The pressure-sensitive adhesive sheet and the liner-attached double-sided pressure-sensitive adhesive sheet may be preferably used as a temporary fixing sheet when processing any appropriate member (for example, an electronic component such as a semiconductor chip). In one embodiment, the liner-attached double-sided pressure-sensitive adhesive sheet may be used as a sheet for temporarily fixing a semiconductor chip when manufacturing a CSP (Chip Size / Scale Package) or a WLP (Wafer Level Package). In one embodiment, the liner-attached double-sided pressure-sensitive adhesive sheet is used in processing including a step in which the second liner is peeled off first. In one embodiment, the semiconductor chip is encapsulated with the encapsulating resin, and the processing temperature during resin encapsulation is 100° C. or higher.

[0073] In one embodiment, the liner-attached double-sided PSA sheet is in a roll form. EXAMPLES

[0074] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" are by weight unless otherwise specified.

[0075] [Production Example 1] Preparation of Acrylic Polymer 1 70 parts of ethyl acrylate, 3 parts of butyl acrylate, 30 parts of 2-ethylhexyl acrylate, 5 parts of methyl methacrylate, 3.5 parts of 2-hydroxyethyl acrylate, and 0.2 parts of benzoyl peroxide as a polymerization initiator were added to toluene, and the mixture was heated to obtain a toluene solution of acrylic polymer 1. Here, 3.1% by weight of the repeating units derived from monomers constituting acrylic polymer 1 were repeating units derived from monomers having an active hydrogen group.

[0076] [Production Example 2] Preparation of Acrylic Polymer 2 50 parts of butyl acrylate, 50 parts of ethyl acrylate, 0.5 parts of acrylic acid, 0.1 parts of 2-hydroxyethyl acrylate, and 0.2 parts of benzoyl peroxide as a polymerization initiator were added to toluene, and then heated to obtain a toluene solution of acrylic polymer 2. Note that 0.60% by weight of the repeating units derived from monomers constituting acrylic polymer 2 here are repeating units derived from monomers having an active hydrogen group.

[0077] [Production Example 3] Preparation of Acrylic Polymer 3 70 parts of methyl acrylate, 2 parts of butyl acrylate, 30 parts of 2-ethylhexyl acrylate, 10 parts of acrylic acid, and 0.2 parts of benzoyl peroxide as a polymerization initiator were added to ethyl acetate, and the mixture was heated to obtain an ethyl acetate solution of acrylic polymer 3. Here, 8.9% by weight of the repeating units derived from monomers constituting acrylic polymer 3 are repeating units derived from monomers having an active hydrogen group.

[0078] [Example 1] A toluene solution of the acrylic polymer 1 (acrylic polymer 1: 100 parts by weight), 3 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), and 10 parts by weight of a plasticizer (manufactured by DIC Corporation, product name "Monocizer W700") were mixed together to prepare a pressure-sensitive adhesive. The above adhesive was coated (applied and dried) on the release-treated surface of a liner (PET film, thickness: 38 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-38") to form an adhesive layer (thickness: 10 μm). The above-mentioned liner with adhesive layer was attached to a substrate (polyester film, manufactured by Toray Industries, product name "Lumirror S10", thickness: 50 μm) to obtain a liner-attached adhesive sheet precursor. The Si-Kα radiation intensity of the liner (product name "MRF-38") was 18 (kcps). The Si-Kα radiation intensity was measured as follows. The liner-attached pressure-sensitive adhesive sheet precursor was left to stand for 5 days in an environment of 40° C. temperature and 20% humidity (humidification and heating step) to obtain a liner-attached pressure-sensitive adhesive sheet consisting of liner / pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer) / substrate. ·Si-Kα line intensity measurement of liner X-ray fluorescence analysis was performed on 100 points randomly selected on the liner surface (release-treated surface). More specifically, the Si-Kα radiation intensity (i) of the surface of the liner in contact with the adhesive layer (the surface coated with a release agent) and the Si-Kα radiation intensity (ii) of the surface not in contact with the adhesive layer (the surface not coated with a release agent) were measured, the absolute value of the value obtained by subtracting the value of (ii) from the value of (i) was calculated, and the average value of the 100 points was taken as the Si-Kα radiation intensity of the liner. The Si-Kα radiation intensity is the intensity at a wavelength of 7.125 angstroms measured using the following device. Equipment: Rigaku ZSX100e Analysis area: 30mmφ Analysis element: Si Analytical crystal: RX4 Output: 50kV, 70mA

[0079] [Example 2] A toluene solution of the above acrylic polymer 1 (acrylic polymer 1:100 parts by weight), 3 parts by weight of a crosslinker (manufactured by Tosoh Corporation, product name "Coronate L"), and 10 parts by weight of a plasticizer (manufactured by DIC Corporation, product name "Monocizer W700") were mixed together to prepare an adhesive. The above adhesive was applied to the release-treated surface of a liner (PET film, thickness: 38 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-38") to form an adhesive layer (thickness: 10 μm). The above liner with adhesive layer was attached to a substrate (polyethylene naphthalate film, manufactured by Teijin DuPont Films, product name "Teonex Q51", thickness: 50 μm) to obtain a liner-attached adhesive sheet precursor. The lined pressure-sensitive adhesive sheet precursor was left to stand for 5 days in an environment of 40° C. temperature and 20% humidity to obtain a lined pressure-sensitive adhesive sheet consisting of liner / pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer) / substrate.

[0080] [Example 3] A toluene solution of the above acrylic polymer 1 (acrylic polymer 1:100 parts by weight), 3 parts by weight of a crosslinker (manufactured by Tosoh Corporation, product name "Coronate L"), and 10 parts by weight of a plasticizer (manufactured by DIC Corporation, product name "Monocizer W700") were mixed together to prepare an adhesive. The above adhesive was applied to the release-treated surface of a liner (PET film, thickness: 38 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-38") to form an adhesive layer (thickness: 10 μm). The above liner with adhesive layer was attached to a substrate (aromatic polyimide film, manufactured by Ube Industries, product name "Upilex-R", thickness: 50 μm) to obtain a liner-attached adhesive sheet precursor. The lined pressure-sensitive adhesive sheet precursor was left to stand for 5 days in an environment of 40° C. temperature and 20% humidity to obtain a lined pressure-sensitive adhesive sheet consisting of liner / pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer) / substrate.

[0081] [Example 4] The above toluene solution of acrylic polymer 1 (acrylic polymer 1:100 parts by weight), 3 parts by weight of a crosslinker (manufactured by Tosoh Corporation, product name "Coronate L"), and 10 parts by weight of a plasticizer (manufactured by DIC Corporation, product name "Monocizer W700") were mixed to prepare adhesive a1. The adhesive a1 was applied to the release-treated surface of a liner (PET film, thickness: 38 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-38") to form an adhesive layer (thickness: 7 μm). The above liner with adhesive layer was attached to a substrate (aromatic polyimide film, manufactured by DuPont, product name "Kapton 200H", thickness: 50 μm) to obtain a liner-attached adhesive sheet precursor. The lined pressure-sensitive adhesive sheet precursor was left to stand for 5 days in an environment of 40° C. temperature and 20% humidity to obtain a lined pressure-sensitive adhesive sheet consisting of liner / pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer) / substrate.

[0082] [Example 5] A pressure-sensitive adhesive sheet with a liner was obtained in the same manner as in Example 4, except that the thickness of the pressure-sensitive adhesive layer was 2 μm.

[0083] [Example 6] A pressure-sensitive adhesive sheet with a liner was obtained in the same manner as in Example 4, except that the thickness of the pressure-sensitive adhesive layer was 15 μm.

[0084] [Example 7] (Adhesive sheet with liner A2) The above toluene solution of acrylic polymer 1 (acrylic polymer 1:100 parts by weight), 3 parts by weight of a crosslinker (manufactured by Tosoh Corporation, product name "Coronate L"), and 10 parts by weight of a plasticizer (manufactured by DIC Corporation, product name "Monocizer W700") were mixed to prepare adhesive a1. The adhesive a1 was applied to the release-treated surface of a liner (PET film, thickness: 38 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-38") to form an adhesive layer (thickness: 7 μm). The above-mentioned liner with adhesive layer was bonded to a substrate (aromatic polyimide film, manufactured by DuPont, product name "Kapton 200H", thickness: 50 μm) to obtain a liner-attached adhesive sheet a2 consisting of liner (first liner) / adhesive layer (first adhesive layer) / substrate. (Adhesive sheet with liner a2 / undercoat layer laminate) The above toluene solution of acrylic polymer 1 (acrylic polymer 1: 100 parts by weight) and 3 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") were mixed together to prepare adhesive b. The adhesive b was applied to the substrate of the liner-attached adhesive sheet a2 to form a laminate consisting of the liner-attached adhesive sheet a2 / undercoat layer (thickness: 13 μm). (Double-sided adhesive sheet with liner b) A composition for forming a second adhesive layer was prepared by mixing a toluene solution of the above acrylic polymer 1 (acrylic polymer 1:100 parts by weight), 1.5 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), 10 parts by weight of a tackifying resin (manufactured by Sumitomo Bakelite Co., Ltd., product name "SUMILITE PR12603"), 30 parts by weight of thermally expandable microspheres (manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd., product name "Matsumoto Microsphere FN-180SSD"), and 0.5 parts by weight of a colorant (manufactured by Dainichiseika Chemicals Co., Ltd., product name "DYMICS SZ7510 Green") The second adhesive layer-forming composition was applied to the release-treated surface of a liner (PET film, thickness: 50 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-50") to form a second adhesive layer (thickness: 35 μm). The Si-Kα radiation intensity of the liner (product name "MRF-50") was 28 (kcps). The liner with the second pressure-sensitive adhesive layer was attached to a laminate consisting of the liner-attached pressure-sensitive adhesive sheet a2 / undercoat layer to obtain a liner-attached double-sided pressure-sensitive adhesive sheet precursor. The liner-attached double-sided adhesive sheet precursor was left to stand for 5 days in an environment with a temperature of 40°C and a humidity of 20% to obtain a liner-attached double-sided adhesive sheet consisting of a first liner / first adhesive layer / substrate / undercoat layer / second adhesive layer / second liner.

[0085] [Example 8] (Adhesive sheet with liner A2) In the same manner as in Example 7, a lined pressure-sensitive adhesive sheet a2 (liner (first liner) / pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer) / substrate) was obtained. (Adhesive sheet with liner a2 / undercoat layer laminate) The above toluene solution of acrylic polymer 1 (acrylic polymer 1: 100 parts by weight) and 3 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") were mixed together to prepare adhesive b. The adhesive b was applied to the substrate of the liner-attached adhesive sheet a2 to form a laminate consisting of the liner-attached adhesive sheet a2 / undercoat layer (thickness: 13 μm). (Double-sided adhesive sheet with liner b') A composition for forming a second adhesive layer was prepared by mixing a toluene solution of the above acrylic polymer 1 (acrylic polymer 1:100 parts by weight), 1.5 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), 10 parts by weight of a tackifying resin (manufactured by Sumitomo Bakelite Co., Ltd., product name "SUMILITE PR12603"), 30 parts by weight of thermally expandable microspheres (manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd., product name "Matsumoto Microsphere FN-180SSD"), and 0.5 parts by weight of a colorant (manufactured by Dainichiseika Chemicals Co., Ltd., product name "DYMICS SZ7510 Green") The composition for forming a second adhesive layer was applied to the release-treated surface of a liner (PET film, thickness: 50 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-50") to form a second adhesive layer (thickness: 35 μm). The liner with the second pressure-sensitive adhesive layer was attached to a laminate consisting of the liner-attached pressure-sensitive adhesive sheet a2 / undercoat layer to obtain a liner-attached double-sided pressure-sensitive adhesive sheet precursor. The liner-attached double-sided adhesive sheet precursor was left to stand for 2 hours in an environment with a temperature of 90°C and a humidity of 1% RH to obtain a liner-attached double-sided adhesive sheet consisting of a first liner / first adhesive layer / substrate / undercoat layer / second adhesive layer / second liner.

[0086] [Example 9] (Adhesive sheet with liner A2) In the same manner as in Example 7, a lined pressure-sensitive adhesive sheet a2 (liner (first liner) / pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer) / substrate) was obtained. (Adhesive sheet with liner a2 / undercoat layer laminate) The above toluene solution of acrylic polymer 1 (acrylic polymer 1: 100 parts by weight) and 3 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") were mixed together to prepare adhesive b. The adhesive b was applied to the substrate of the liner-attached adhesive sheet a2 to form a laminate consisting of the liner-attached adhesive sheet a2 / undercoat layer (thickness: 13 μm). (Double-sided adhesive sheet with liner b'') A composition for forming a second adhesive layer was prepared by mixing a toluene solution of the above acrylic polymer 1 (acrylic polymer 1:100 parts by weight), 1.5 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), 10 parts by weight of a tackifying resin (manufactured by Sumitomo Bakelite Co., Ltd., product name "SUMILITE PR12603"), 60 parts by weight of thermally expandable microspheres (manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd., product name "Matsumoto Microsphere FN-180SSD"), and 0.5 parts by weight of a colorant (manufactured by Dainichiseika Chemicals Co., Ltd., product name "DYMICS SZ7510 Green") The composition for forming a second adhesive layer was applied to the release-treated surface of a liner (PET film, thickness: 50 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-50") to form a second adhesive layer (thickness: 35 μm). The liner with the second pressure-sensitive adhesive layer was attached to a laminate consisting of the liner-attached pressure-sensitive adhesive sheet a / undercoat layer to obtain a liner-attached double-sided pressure-sensitive adhesive sheet precursor. The liner-attached double-sided adhesive sheet precursor was left to stand for 3 days in an environment with a temperature of 40°C and a humidity of 92% RH to obtain a liner-attached double-sided adhesive sheet consisting of a first liner / first adhesive layer / substrate / undercoat layer / second adhesive layer / second liner.

[0087] [Example 10] (A3 adhesive sheet with liner) The above toluene solution of acrylic polymer 2 (acrylic polymer 2: 100 parts by weight), 3 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), and 15 parts by weight of a tackifying resin (manufactured by Arakawa Chemical Industries, Ltd., product name "Tamanol 200N") were mixed to prepare adhesive a'. The above adhesive a' was applied to the release-treated surface of a liner (PET film, thickness: 38 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-38") to form an adhesive layer (thickness: 5 μm). The above-mentioned liner with adhesive layer was bonded to a substrate (aromatic polyimide film, manufactured by DuPont, product name "Kapton 200H", thickness: 50 μm) to obtain a liner-attached adhesive sheet a3 consisting of liner (first liner) / adhesive layer (first adhesive layer) / substrate. (Adhesive sheet with liner A3 / undercoat layer laminate) The above toluene solution of acrylic polymer 2 (acrylic polymer 2: 100 parts by weight) and 3 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") were mixed together to prepare adhesive b'. The adhesive b' was applied to the base material of the liner-attached adhesive sheet a3 to form a laminate consisting of the liner-attached adhesive sheet a3 / undercoat layer (thickness: 13 μm). (B2 double-sided adhesive sheet with liner) A composition for forming a second adhesive layer was prepared by mixing the above toluene solution of acrylic polymer 2 (acrylic polymer 2: 100 parts by weight), 1.5 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), 10 parts by weight of a tackifying resin (manufactured by Sumitomo Bakelite Co., Ltd., product name "SUMILITE PR12603"), 30 parts by weight of thermally expandable microspheres (manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd., product name "Matsumoto Microsphere FN-180SSD"), and 0.5 parts by weight of a colorant (manufactured by Dainichiseika Chemicals Co., Ltd., product name "DYMICS SZ7510 Green") The composition for forming a second adhesive layer was applied to the release-treated surface of a liner (PET film, thickness: 50 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-50") to form a second adhesive layer (thickness: 35 μm). The second pressure-sensitive adhesive layer-attached liner and a laminate consisting of the liner-attached pressure-sensitive adhesive sheet a3 / undercoat layer were attached to each other to obtain a liner-attached double-sided pressure-sensitive adhesive sheet precursor. The liner-attached double-sided adhesive sheet precursor was left to stand for 5 days in an environment of 40°C temperature and 20% RH humidity to obtain a liner-attached double-sided adhesive sheet consisting of a first liner / first adhesive layer / substrate / undercoat layer / second adhesive layer / second liner.

[0088] [Example 11] (A4 adhesive sheet with liner) The above toluene solution of acrylic polymer 3 (acrylic polymer 3: 100 parts by weight), 3 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), and 15 parts by weight of a tackifying resin (manufactured by Arakawa Chemical Industries, Ltd., product name "Tamanol 200N") were mixed together to prepare adhesive a''. The above adhesive a' was applied to the release-treated surface of a liner (PET film, thickness: 38 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-38") to form an adhesive layer (thickness: 5 μm). The above-mentioned liner with adhesive layer was bonded to a substrate (aromatic polyimide film, manufactured by DuPont, product name "Kapton 200H", thickness: 50 μm) to obtain a liner-attached adhesive sheet a4 consisting of liner (first liner) / adhesive layer (first adhesive layer) / substrate. (A4 adhesive sheet with liner / undercoat layer laminate) The above toluene solution of acrylic polymer 3 (acrylic polymer 3: 100 parts by weight) and 3 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") were mixed together to prepare adhesive b''. The adhesive b'' was applied to the base material of the liner-attached adhesive sheet a4 to form a laminate consisting of the liner-attached adhesive sheet a4 / undercoat layer (thickness: 13 μm). (B3 double-sided adhesive sheet with liner) A composition for forming a second adhesive layer was prepared by mixing the above toluene solution of acrylic polymer 3 (acrylic polymer 3: 100 parts by weight), 1.5 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), 10 parts by weight of a tackifying resin (manufactured by Sumitomo Bakelite Co., Ltd., product name "SUMILITE PR12603"), 30 parts by weight of thermally expandable microspheres (manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd., product name "Matsumoto Microsphere FN-180SSD"), and 0.5 parts by weight of a colorant (manufactured by Dainichiseika Chemicals Co., Ltd., product name "DYMICS SZ7510 Green") The composition for forming a second adhesive layer was applied to the release-treated surface of a liner (PET film, thickness: 50 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-50") to form a second adhesive layer (thickness: 35 μm). The liner with the second adhesive layer was attached to a laminate consisting of the liner-attached adhesive sheet a4 / undercoat layer to obtain a liner-attached double-sided adhesive sheet precursor. The liner-attached double-sided adhesive sheet precursor was left to stand for 5 days in an environment of 40°C temperature and 20% RH humidity to obtain a liner-attached double-sided adhesive sheet consisting of a first liner / first adhesive layer / substrate / undercoat layer / second adhesive layer / second liner.

[0089] [Comparative Example 1] The above toluene solution of acrylic polymer 1 (acrylic polymer 1:100 parts by weight), 3 parts by weight of a crosslinker (manufactured by Tosoh Corporation, product name "Coronate L"), and 10 parts by weight of a plasticizer (manufactured by DIC Corporation, product name "Monocizer W700") were mixed to prepare adhesive a1. The above adhesive a was applied to the release-treated surface of a liner (PET film, thickness: 38 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-38") to form an adhesive layer (thickness: 7 μm). The above liner with adhesive layer was attached to a substrate (aromatic polyimide film, manufactured by DuPont, product name "Kapton 200H", thickness: 50 μm) to obtain a liner-attached adhesive sheet precursor. The liner-attached pressure-sensitive adhesive sheet precursor was left to stand for 4 hours in an environment at a temperature of 200° C. and a humidity of 0.1% RH to obtain a liner-attached pressure-sensitive adhesive sheet consisting of a liner / pressure-sensitive adhesive layer (first pressure-sensitive adhesive layer) / substrate.

[0090] [Comparative Example 2] (Adhesive sheet with liner A2) The above toluene solution of acrylic polymer 1 (acrylic polymer 1:100 parts by weight), 3 parts by weight of a crosslinker (manufactured by Tosoh Corporation, product name "Coronate L"), and 10 parts by weight of a plasticizer (manufactured by DIC Corporation, product name "Monocizer W700") were mixed to prepare adhesive a1. The above adhesive a was applied to the release-treated surface of a liner (PET film, thickness: 38 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-38") to form an adhesive layer (thickness: 7 μm). The above-mentioned liner with adhesive layer was bonded to a substrate (aromatic polyimide film, manufactured by DuPont, product name "Kapton 200H", thickness: 50 μm) to obtain a liner-attached adhesive sheet a2 consisting of liner (first liner) / adhesive layer (first adhesive layer) / substrate. (Adhesive sheet with liner a2 / undercoat layer laminate) The above toluene solution of acrylic polymer 1 (acrylic polymer 1: 100 parts by weight) and 3 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L") were mixed together to prepare adhesive b. The adhesive b was applied to the substrate of the liner-attached adhesive sheet a2 to form a laminate consisting of the liner-attached adhesive sheet a2 / undercoat layer (thickness: 13 μm). (Adhesive sheet with liner) A composition for forming a second adhesive layer was prepared by mixing a toluene solution of the above acrylic polymer 1 (acrylic polymer 1:100 parts by weight), 1.5 parts by weight of a crosslinking agent (manufactured by Tosoh Corporation, product name "Coronate L"), 10 parts by weight of a tackifying resin (manufactured by Sumitomo Bakelite Co., Ltd., product name "SUMILITE PR12603"), 30 parts by weight of thermally expandable microspheres (manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd., product name "Matsumoto Microsphere FN-180SSD"), and 0.5 parts by weight of a colorant (manufactured by Dainichiseika Chemicals Co., Ltd., product name "DYMICS SZ7510 Green") The composition for forming a second adhesive layer was applied to the release-treated surface of a liner (PET film, thickness: 50 μm, silicone-based release-treated product, manufactured by Mitsubishi Plastics, Inc., product name "MRF-50") to form a second adhesive layer (thickness: 35 μm). The liner with the second pressure-sensitive adhesive layer was attached to a laminate consisting of the liner-attached pressure-sensitive adhesive sheet a2 / undercoat layer to obtain a liner-attached double-sided pressure-sensitive adhesive sheet precursor. The liner-attached double-sided adhesive sheet precursor was left to stand for 7 days in an environment with a temperature of 85°C and a humidity of 92% RH to obtain a liner-attached double-sided adhesive sheet consisting of a first liner / first adhesive layer / substrate / undercoat layer / second adhesive layer / second liner.

[0091] [evaluation] The pressure-sensitive adhesive sheets obtained in the examples and comparative examples were subjected to the following evaluations, and the results are shown in Table 1. (1) Adhesive strength The first liner was peeled off from the liner-attached adhesive sheets obtained in the Examples and Comparative Examples, and the adhesive sheets were cut to a size of 20 mm wide and 140 mm long. A polyethylene terephthalate film (manufactured by Toray Industries, product name "Lumirror S-10", thickness: 25 μm, width: 20 mm) was then bonded to the first adhesive layer by rolling a 2 kg roller back and forth once in accordance with JIS Z 0237 (2000) in an atmosphere of temperature: 23°C and humidity: 65 RH to prepare an evaluation sample. The evaluation sample was set in a tensile tester with a thermostatic chamber set at 23° C. (manufactured by Shimadzu Corporation, product name "Shimadzu Autograph AG-120kN") and left for 30 minutes. After leaving it, the load was measured when the polyethylene terephthalate was peeled off from the adhesive sheet at a temperature of 23°C under conditions of a peel angle of 180° and a peel speed (tensile speed) of 300 mm / min. The maximum load at that time (the maximum load excluding the peak top at the initial stage of measurement) was calculated, and this maximum load was recorded as the adhesive strength (N / 20 mm). (2) Moisture content The liners were peeled off from the liner-attached pressure-sensitive adhesive sheets obtained in the Examples and Comparative Examples, and the moisture content of the pressure-sensitive adhesive sheets was measured by Karl Fischer titration. Details of the measuring device and measuring conditions are as follows. Measuring device: Coulometric titration moisture measuring device (manufactured by Mitsubishi Chemical Corporation, CA-06), heating vaporization device (manufactured by Mitsubishi Chemical Corporation, VA-06) Measurement conditions: Thermal vaporization method (heated to 150°C) Anolyte: Aquamicron AKX (manufactured by API Corporation) Catholyte: Aquamicron CXU (manufactured by API Corporation) (3) Contact angle The first liner was peeled off from the liner-attached pressure-sensitive adhesive sheets obtained in the Examples and Comparative Examples, and the contact angle of water on the first pressure-sensitive adhesive layer was measured. Using a contact angle meter (manufactured by Kyowa Interface Co., Ltd., product name "CX-A Type"), 2 μl of pure water was dropped onto the surface of the first adhesive layer in an environment of 23°C / 50% RH, and the contact angle of the droplet was measured 5 seconds after the drop was dropped, and the average value was calculated. (4) Gel fraction 0.1 g of the first adhesive layer was wrapped in a mesh sheet and left to stand in 50 ml of toluene at room temperature for one week to allow the sample to be immersed in toluene. After that, the toluene-insoluble matter was taken out and dried at 70° C. for 2 hours, and then the dried toluene-insoluble matter was weighed. The gel fraction of the resin layer was calculated from the weight of the sample before immersion in toluene and the weight of the toluene-insoluble matter according to the following formula. Gel fraction (%) = [(weight of toluene insoluble matter) / (weight of sample before immersion in toluene)] × 100 (5) Evaluation of fluidity of encapsulating resin precursor The liner was peeled off from the liner-attached pressure-sensitive adhesive sheets obtained in the Examples and Comparative Examples, and the second pressure-sensitive adhesive layer side was attached to a glass plate. A 130 μm thick polytetrafluoroethylene (PTFE) sheet with a 3 mm diameter hole was placed on the first pressure-sensitive adhesive layer. A sealing resin precursor (epoxy resin, Nagase ChemteX Corporation, product name "R4212") was poured into the hole of the PTFE sheet to form a columnar body of the sealing resin precursor with a diameter of 3 mm and a thickness of 130 μm. The PTFE sheet was removed, and the adhesive sheet with the pillars of the encapsulating resin precursor was placed on an optical microscope equipped with a hot stage as a sample. After being left at 23°C for 1 minute, the sample was heated to 130°C. For the sealing resin precursor that flows when heated, the time required for the shortest distance between the outer edge of the position where the columns were formed and the outer edge of the sealing resin precursor after it had flowed to become 30 μm was measured. The above measurement was carried out 10 times, and the variation in the fluidity of the encapsulating resin precursor was evaluated according to the following criteria based on the difference between the longest time and the shortest time. Excellent (〇 in the table): The difference above is less than 60 seconds Acceptable (△ in the table): The difference between the above is 60 seconds to 180 seconds Not possible (X in the table): The difference above exceeds 180 seconds

[0092] [Table 1] [Explanation of symbols]

[0093] 10 Base material 20 Adhesive layer 30 Second adhesive layer 100, 200 Adhesive Sheet

Claims

1. A pressure-sensitive adhesive sheet comprising a substrate and a pressure-sensitive adhesive layer disposed on at least one side of the substrate, The adhesive strength of the pressure-sensitive adhesive layer when attached to polyethylene terephthalate at 23°C is 0.1 N / 20 mm to 8 N / 20 mm; The adhesive layer is made of an adhesive containing a base polymer, and the base polymer has an sp value of 7 (cal / cm 3 ) 1/2 ~10(cal / cm 3 ) 1/2 and The pressure-sensitive adhesive layer has a water contact angle of 70° to 120°. The moisture content of the pressure-sensitive adhesive sheet is 0.5% by weight to 6% by weight. Adhesive sheet.

2. 2. The pressure-sensitive adhesive sheet according to claim 1, wherein the substrate is a resin sheet made of a resin having a glass transition temperature (Tg) of 60°C to 450°C.

3. The pressure-sensitive adhesive sheet according to claim 1 , wherein the substrate is made of an aromatic polyimide resin.

4. The pressure-sensitive adhesive sheet according to any one of claims 1 to 3, wherein the pressure-sensitive adhesive layer has a thickness of 2 µm to 15 µm.

5. The pressure-sensitive adhesive sheet according to any one of claims 1 to 4, wherein the pressure-sensitive adhesive layer has a gel fraction of 60% to 100%.

6. the base polymer is an acrylic polymer, the acrylic polymer contains a structural unit derived from a hydroxyl group-containing monomer, 6. The pressure-sensitive adhesive sheet according to claim 1, wherein the content of the structural unit derived from the hydroxyl group-containing monomer is 0.1 to 20 parts by weight based on 100 parts by weight of all structural units constituting the acrylic polymer.

7. The pressure-sensitive adhesive sheet according to claim 1 , further comprising a second pressure-sensitive adhesive layer on the opposite side of the substrate to the pressure-sensitive adhesive layer.

8. The pressure-sensitive adhesive sheet according to claim 1 , which is used as a sheet for temporarily fixing a semiconductor chip during the manufacture of a CSP (Chip Size / Scale Package) or a WLP (Wafer Level Package).

9. The pressure-sensitive adhesive sheet according to claim 8 , wherein the semiconductor chip is sealed with a sealing resin, and the processing temperature during the resin sealing is 100° C. or higher.

10. forming a coating layer of a composition containing a pressure-sensitive adhesive on a substrate; placing a liner on the coating layer surface to form a laminate; and a humidification and heating step of placing the laminate in an environment in which the humidification and heating time, temperature, and humidity are controlled, In the humidification and heating process, the product of the humidification and heating time, temperature and humidity is 100 to 300,000 ° C. RH% h. A method for producing the pressure-sensitive adhesive sheet according to claim 1 .

Citation Information

Patent Citations

  • Chip-shaped electronic component and its manufacturing method, and pseudo wafer used for manufacturing method of chip-shaped electronic component and its manufacturing method

    JP2001308116A

  • Chip-shaped electronic component and its manufacturing method, and pseudo-wafer used for manufacture of chip- shaped electronic component and its manufacturing method

    JP2001313350A

  • Insulating tape

    JP2012102229A

  • Pressure sensitive adhesive sheet

    JP2015168711A

  • Adhesive composition, and adhesive sheet

    JP2018016701A