Semiconductor device manufacturing method
The use of an organic gas with electron-donating atoms forms a thermally stable organometallic complex, addressing inefficiencies in complex gas systems and foreign matter generation in semiconductor etching, thereby improving processing efficiency and reducing cycle times.
Patent Information
- Application Number
- JP2023553024
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-08-23
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2042-08-23
AI Technical Summary
Existing semiconductor etching techniques require complex gas supply systems and result in inefficient processing due to the use of multiple gases, leading to longer cycle times and potential thermal instability of organometallic complexes, which can decompose and adhere as foreign matter.
A method involving the use of an organic gas with electron-donating atoms in its molecule to form a thermally stable organometallic complex, allowing for efficient etching by neutralizing the metal film's charge and facilitating high volatility without the need for a complicated gas supply system.
This approach ensures efficient processing with reduced foreign substance generation by stabilizing the organometallic complex, eliminating the need for a complex gas supply system and enhancing etching efficiency.
Smart Images

Figure 0007568870000001 
Figure 0007568870000002 
Figure 0007568870000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for manufacturing a semiconductor device and a semiconductor manufacturing apparatus. [Background technology]
[0002] The demand for cutting-edge semiconductor devices to be smaller, faster, more powerful, and more energy efficient is accelerating. New materials are increasingly being adopted, and there is a demand for these materials to be processed (e.g., by deposition and etching) with ultra-high precision at the nanometer level.
[0003] An example of such a technique is disclosed in JP-A-2018-500767 (Patent Document 1). In Patent Document 1, in order to process Al2O3, HfO2, and ZrO2 films with ultra-high precision at the atomic layer level, a reactive gas containing halogen such as F (fluorine) is reacted with the film to be processed to convert it into a fluoride, which is then reacted with an organometallic compound that serves as a ligand exchange agent to convert it into a volatile organometallic complex. , organometallic complexes More specifically, in the case of an Al2O3 film, the AlF is removed by reacting it with a reactive gas containing F. x (fluoride) and reacting with a ligand exchanger, trialkylaluminum, to give Al(CH3)F x-1 and heated to 200℃~300℃ Al(CH 3 )F x-1 of This series of processes allows the Al2O3 film to be etched with high precision at the atomic layer level. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Special Publication No. 2018-500767 [Non-patent literature]
[0005] [Non-Patent Document 1] Younger Lee and Steven M. George, Journal of Vacuum Science & Technology A 36(6) 061504 (2018) Summary of the Invention [Problem to be solved by the invention]
[0006] In the course of studying ultra-high-precision processing of materials containing various elements at the nanometer level, the inventors of the present application have been studying the application of the technique to multilayer films in which many different materials are laminated in multiple layers. As a result of such studies, the inventors have determined that there is a need for an etching technique that can be performed at relatively low temperatures in order to prevent interlayer diffusion in multilayer films.
[0007] The above-mentioned Patent Document 1 is considered to be a promising technology from the viewpoint of realizing selective etching at or below 400° C. However, as a result of investigation, it is considered that there is room for improvement in the following points.
[0008] Specifically, since two completely different gases, an F-containing reactive gas and a ligand exchange agent, are used, the gas supply system for supplying the gases and its control become complicated, and there is a risk that the etching processing apparatus will become large-sized or expensive.
[0009] In addition, between the treatment with the F-containing reactive gas and the treatment with the ligand exchange agent, a period of time must be provided to pause the reaction by replacing the gas in the chamber in order to prevent the two types of gases from mixing. Furthermore, a reaction induction period must be provided between the pause of the first reaction and the start of the second reaction. Thus, even if the supply of the first gas is stopped and the supply of the second gas is started, the second reaction cannot be started immediately, and as a result, the cycle time may be lengthened and the etching efficiency may be reduced.
[0010] In addition, the volatile organometallic complexes produced by the ligand exchange reaction are usually not very thermally stable. Therefore, after volatilization from the wafer surface, a part of the complexes may thermally decompose and become foreign matter while being discharged from the chamber, which may remain in the processing chamber and reattach to the wafer surface. This point was not sufficiently taken into consideration in the above-mentioned conventional techniques.
[0011] An object of the present invention is to provide a method for manufacturing a semiconductor device that does not require a complicated gas supply system, ensures processing efficiency, and suppresses the generation of foreign matter. and The object of the present invention is to provide a semiconductor manufacturing device. [Means for solving the problem]
[0012] In order to solve the above problems, one representative method for manufacturing a semiconductor device of the present invention includes a step of comparing a remaining amount of processing of a film to be processed formed on a semiconductor wafer with a threshold value, a step of heating the semiconductor wafer while supplying an organic gas containing a substance having at least two substituents having an unshared electron pair in its molecule, to form a compound of the film to be processed and the organic gas, and a step of further heating the semiconductor wafer after the step of forming the compound based on the result of the comparison, thereby raising the temperature to a predetermined temperature and desorbing the compound from the surface of the semiconductor wafer.
[0013] Furthermore, one representative semiconductor manufacturing apparatus of the present invention is a semiconductor manufacturing apparatus including a vacuum vessel having a processing chamber therein, a stage on which a semiconductor wafer having a film to be processed arranged inside the processing chamber and on its surface is placed, a processing gas supply unit that supplies an organic gas into the processing chamber, an exhaust unit that evacuates the processing chamber, a heater that heats the semiconductor wafer to a predetermined temperature, and a control unit, wherein the organic gas has at least two substituents having an unshared electron pair in its molecule, and the control unit controls the steps of: comparing a processing remaining amount of the film to be processed with a threshold value; heating the semiconductor wafer while supplying an organic gas containing a substance having at least two substituents having an unshared electron pair in its molecule to the processing chamber to form a compound of the film to be processed and the organic gas; and, based on the result of the comparison, further heating the semiconductor wafer after the compound forming step to a predetermined temperature to desorb the compound from the surface of the semiconductor wafer. Effect of the Invention
[0014] According to the present invention, it is possible to provide a semiconductor device manufacturing method or semiconductor manufacturing apparatus that can ensure processing efficiency and suppress the generation of foreign matter without requiring a complex gas supply system. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a diagram illustrating a schematic configuration of a semiconductor manufacturing apparatus according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a flow chart showing wafer processing performed in the semiconductor manufacturing equipment. [Diagram 3] FIG. 3 is a diagram showing a time chart of the process B including steps S103B to S106B. [Figure 4] FIG. 4 is a diagram showing a time chart of the process A including steps S103A to S107A. [Diagram 5] FIG. 5 is a diagram showing a time chart of a modified example performed in a semiconductor manufacturing apparatus. [Figure 6]FIG. 6 shows the molecular structures of the components of the complexing gas. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The inventors have discovered a phenomenon in which a highly thermally stable and highly volatile organometallic complex is generated in one step by exposing a film to be etched to an organic gas having electron donor atoms at at least two positions in the molecule. The inventors have discovered that this phenomenon can be utilized to achieve highly efficient etching.
[0017] In an organic gas containing an organic compound having electron-donating atoms at at least two positions in the molecule, the electron-donating atoms donate electrons to the positive charges of the metal elements in the film to be etched, forming a thermally stable organometallic complex having strong electron-donating and back-donating coordinate bonds. By adopting such an organometallic complex, the present invention can solve the thermal instability of the organometallic complex, which is a problem of the above-mentioned conventional technology.
[0018] In the organometallic complex of the embodiment, the positive charges of the metal elements of the film to be etched are neutralized by electrons donated by two electron donating atoms in the etching gas. When the charges are neutralized in this way, the electrostatic charge acting between adjacent molecules is reduced. adsorption This eliminates the need for the organic gas to be etched, and the volatility (sublimability) of the organometallic complex is increased. In addition, since a highly volatile organometallic complex can be produced in a single step by exposing the film to be etched to the organic gas, it is no longer necessary to provide a reaction pause, as was used in conventional techniques, and as a result, a decrease in etching efficiency can be avoided.
[0019] [Embodiment] Hereinafter, an embodiment of the present invention will be described with reference to Figures 1 to 6. However, the present invention is not limited to this embodiment.
[0020] (Device Configuration) FIG. 1 is a diagram illustrating a schematic configuration of a semiconductor manufacturing apparatus according to an embodiment of the present invention.
[0021] The processing chamber 1 is composed of a base chamber 11, which is a cylindrical metal container. Inside the base chamber 11, a wafer stage (hereinafter also referred to as "stage") 4 is installed on which a semiconductor wafer (hereinafter also referred to as "wafer") 2, which is a sample to be processed, is placed. In order to generate plasma using an ICP (Inductively Coupled Plasma) discharge method, a plasma generation unit is installed above the processing chamber 1, which is composed of a quartz chamber 12, an ICP coil 34 arranged outside the quartz chamber 12, and a high-frequency power supply 20.
[0022] In the present invention, it is not necessary to use ICP plasma, so the present invention can be applied to a configuration that omits the plasma generation unit. However, it is assumed that a process using ICP plasma, such as ALD (Atomic Layer Deposition) processing that stacks atomic layers or ALE (Plasma Enhanced Atomic Layer Etching) processing that uses plasma, will be performed in a process before or after the process that the present invention targets. For this reason, a configuration including an ICP plasma generation unit will be described as shown in FIG. 1.
[0023] A high frequency power supply 20 for generating plasma is connected to the ICP coil 34 via a matching box 22, and a frequency band of several tens of MHz is used for the frequency of the high frequency power supply 20. A top plate 6, a shower plate 5, and a gas dispersion plate 17 are provided on the upper part of the quartz chamber 12. Gas (processing gas) supplied for processing the wafer 2 is introduced into the processing chamber 1 through a gap on the outer periphery of the gas dispersion plate 17.
[0024] In this embodiment, the flow rate of the process gas is adjusted by mass flow controllers 50-1 to 50-3 arranged in the integrated mass flow controller control unit 51. The process gas contains a plurality of gas species, and a mass flow controller 50-1 to 50-3 is provided for each gas species. In FIG. 1, the supply of three types of process gas, Ar, O2, and H2, is controlled by the corresponding mass flow controllers 50-1, 50-2, and 50-3, respectively. Other process gases, such as hydrofluorocarbon CHF x and chlorocarbon CHCl x 1 also includes a mass flow controller 50-4 that adjusts the flow rate of the He cooling gas supplied between the back surface of the wafer 2 and the upper surface of the dielectric film of the stage 4 on which the wafer 2 is placed. The mass flow controller 50-4 may be provided separately from the integrated mass flow controller control unit 51.
[0025] In this embodiment, an organic gas is used as at least a part of the process gas. The organic gas can be obtained by vaporizing a liquid source using an organic gas vaporizer 47. A tank 45 for storing a liquid chemical 44, which is a liquid raw material, is provided inside the organic gas vaporizer supply 47. The liquid chemical 44 is heated by a heater 46 provided around the tank 45, and the upper part of the tank 45 is filled with vapor of the liquid chemical 44. An atomizer or bubbler may be provided as necessary, but when providing them, care should be taken to prevent foreign matter caused by aerosol fine particles from accumulating inside the processing chamber 1. For example, an operation recipe for cleaning the inside of the processing chamber 1 is prepared in advance, and the recipe is executed periodically.
[0026] The chemical liquid 44 is a liquid that is a raw material for an organic etching gas. The vapor of the chemical liquid 44 is injected into the processing chamber 1 while being controlled by a mass flow controller 50-5 to have a desired flow rate and speed. When the vapor of the chemical liquid 44 is not being introduced into the processing chamber 1, the valves 53 and 54 are closed to isolate the tank 45 from the processing chamber 1. The piping through which the vapor of the chemical liquid 44 flows is heated or insulated as necessary to prevent the vapor of the chemical liquid 44 from condensing on the inner wall surface, and a purge gas is circulated as necessary.
[0027] In addition, the piping between the mass flow controller 50-5 and the processing chamber 1 is appropriately In By monitoring the temperature and pressure, it is possible to detect signs of condensation of the steam and adjust the heating conditions as necessary. organic steaming Kiga Molecules of sulphur are adsorbed. storage In order to prevent the piping from corroding due to the vaporization, a gas purge mechanism (not shown) is provided that, after the process of supplying the vapor of chemical liquid 44 from mass flow controller 50-5 to processing chamber 1 is completed, causes vapor of an inert gas such as Ar or a solvent capable of dissolving chemical liquid 44 to flow through the piping through which the vapor of chemical liquid 44 flows to expel residual gas, and a mechanism (not shown) is provided for maintaining the inside of the piping at a vacuum after the gas purge. These mechanisms (gas purge mechanism and vacuum mechanism) can minimize adverse effects on the processing of the next wafer even if the vapor of chemical liquid 44 condenses or dews in the piping.
[0028] Although the case where the chemical liquid 44 is used has been described, the liquid raw material may not only be liquid at room temperature, but also may be a liquefied raw material obtained by melting and liquefying a solid, or by dissolving and liquefying the raw material in a solvent or the like. In the case of a liquefied raw material obtained by melting and liquefying a solid, it can be easily vaporized by turning it into extremely fine particles using an atomizer, and it is easy to use high-concentration vapor. In addition, in the case of a liquefied raw material obtained by dissolving and liquefying the raw material in a solvent or the like, the pressure after vaporization is the sum of the vapor pressure of the raw material and the vapor pressure of the solvent, and by utilizing this property, To Therefore, the supply concentration of the active ingredient in the treatment gas can be easily adjusted.
[0029] A vacuum exhaust pipe 16 for reducing the pressure in the processing chamber 1 is provided at the bottom of the processing chamber 1. The vacuum exhaust pipe 16 is connected to a pump 15. The pump 15 is, for example, a turbo molecular pump, a mechanical booster pump, a dry pump, or a combination of these. The pressure adjustment mechanism 14 adjusts the flow rate of gas and the like discharged from the processing chamber 1 by increasing or decreasing the flow path cross-sectional area of the vacuum exhaust pipe 16. The pressure adjustment mechanism 14 is, for example, composed of a plurality of plate-like flaps arranged with an axis in a direction transverse to the flow path and rotating around the axis, or a plate member moving inside the flow path transverse to the axial direction of the flow path.
[0030] An IR (Infra-red) lamp unit for heating the wafer 2 is installed between the stage 4 and the quartz chamber 12. The IR lamp unit includes IR lamps 62 arranged in a ring shape above the stage 4, a reflector 63 arranged to cover the IR lamps 62 in order to reflect the light emitted from the IR lamps 62 downward, and an IR light transmitting window 74.
[0031] The IR lamps 62 in this embodiment are multiple circular lamps arranged horizontally concentrically or spirally around the central axis in the vertical direction of the base chamber 11 or the cylindrical stage 4. The arrangement of the IR lamps 62 is not limited to this as long as the wafer heating described later can be realized. In this embodiment, light in a wavelength band from visible light to infrared light is used, and this light is called IR light. In the configuration shown in FIG. 1, IR lamps 62-1, 62-2, and 62-3 are installed around the quartz chamber 12 as the IR lamps 62, which are arranged in three revolutions. The number of IR lamps 62 is not limited to three revolutions, and may be, for example, two or four revolutions.
[0032] An IR lamp power supply 64 is connected to the IR lamp 62. The IR lamp power supply 64 has a function of independently controlling the power supplied to the IR lamps 62-1, 62-2, and 62-3, and adjusts the amount of heat when the wafer 2 is heated.
[0033] The gas flow passage 75 is arranged so as to be surrounded by the IR lamp unit. The process gas, the supply of which is controlled by the mass flow controllers 50 (50-1 to 50-3 and 50-5), flows from the quartz chamber 12 to the process chamber 1 through the gas flow passage 75. The gas flow passage 75 is provided with a slit plate (ion shielding plate) 78 having a plurality of through holes for shielding ions and electrons from among the components of the plasma generated in the quartz chamber 12 and allowing only neutral gas and neutral radicals to pass through. When plasma is not used, the process gas is a neutral gas that does not contain ions or electrons, and therefore the slit plate 78 functions as a flow straightening plate for straightening the flow of the process gas.
[0034] The dimensions and arrangement of the through holes are optimized so that the processing gas is appropriately preheated when the processing gas passes through the through holes of the slit plate 78. Furthermore, the installation location of the slit plate 78 is arranged in consideration of the position of the IR lamp unit so that the preheating function can be exerted.
[0035] A coolant flow path 39 for cooling the stage 4 is formed inside the stage 4. A chiller 38 supplies the coolant and circulates the coolant inside the flow path 39. In addition, an electrostatic adsorption electrode 30 for electrostatically adsorbing the wafer 2 is embedded in the stage 4, and an electrostatic adsorption power supply 31 is connected to the electrostatic adsorption electrode 30.
[0036] In addition, in order to improve the cooling efficiency of the wafer 2, He gas is supplied between the back surface of the wafer 2 placed on the stage 4 and the stage 4. The He gas passes through supply pipes provided inside and on the top surface of the stage 4, and is introduced from an opening on the top surface of the stage 4 into the gap between the back surface of the wafer 2 and the top surface of the stage 4.
[0037] When heating or cooling is performed with the wafer 2 adsorbed, there is a risk that the backside of the wafer 2 will be scratched due to the difference in thermal expansion coefficient between the wafer 2 and the stage 4. For this reason, at least the wafer mounting surface of the stage 4 is coated with a corrosion-resistant resin coating to prevent scratches from occurring on the backside of the wafer 2. The coating applied to the wafer mounting surface of the stage 4 also functions to prevent the stage 4 from being attacked by the process gas or its plasma, radicals, etc.
[0038] Moreover, a thermocouple 70 for measuring the temperature of the stage 4 is installed inside the stage 4. The thermocouple 70 is connected to a thermocouple thermometer 71.
[0039] As another means for measuring the temperature of the wafer 2, optical fibers 92-1 and 92-2 may be installed at three locations, namely, near the center of the stage 4, near the middle in the radial direction, and near the outer periphery in the radial direction. The optical fiber 92-1 is installed to pass through the inside of the stage 4, and guides external IR light output from an external IR light source 93 to the rear surface of the wafer 2 to irradiate the rear surface of the wafer 2.
[0040] On the other hand, the optical fiber 92-2 collects the IR light that is transmitted through and reflected by the wafer 2 among the IR light irradiated by the optical fiber 92-1, and transmits it to a spectrometer 96. The external IR light generated by the external IR light source 93 is branched into multiple optical paths via an optical path switch 94 and an optical distributor 95 (see FIG. 1 3 Light road The light is then irradiated to respective positions on the rear surface of the wafer 2 via separate optical fibers 92-1 for each optical path.
[0041] The IR light absorbed or reflected by the wafer 2 is captured by the optical fiber 92-2 and transmitted to the spectrometer 96. The detector 97 detects data on the spectral intensity distribution (spectral spectrum) for each wavelength band. The spectral data is sent to the calculation unit 41 of the control unit 40 and used to obtain the temperature of the wafer 2 through a predetermined calculation process. In addition, by using a mechanism for switching which measurement point on the wafer is to be spectroscopically measured, the temperature at each location can be obtained.
[0042] Needless to say, the optical fiber used here is tightly sealed with packing or the like so as not to be damaged by the process gas or its plasma, radicals, etc. supplied via the mass flow controllers 50-1, 50-2, 50-3, 50-5. However, it is preferable to use an optical fiber material that is less likely to react with the supplied process gas or its plasma, radicals, etc., so that the measurement capability does not immediately decrease even if the packing of the sealing part deteriorates and the seal leaks due to continued use of the semiconductor manufacturing apparatus of the present invention. For example, when the process gas supplied from the mass flow controller 50-5 contains F (fluorine) atoms, it may be preferable to use a hollow fiber instead of a quartz fiber.
[0043] The control unit 40 controls the on (with output) and off (without output) of the high frequency power supply from the high frequency power source 20 to the ICP coil 34. The control unit 40 also controls the integrated mass flow controller control unit 51 and the organic gas vaporizer supply unit 47 so that gas is supplied to the quartz chamber 12 according to a timing determined by a desired time chart (details of which will be described later). The control unit 40 further controls the vacuum exhaust pipe 16 and the pump 15 to adjust the inside of the processing chamber 1 to be within a desired pressure range.
[0044] The control unit 40 also fixes the wafer 2 on the stage 4, and controls heating and cooling so that the wafer 2 has a desired temperature and temperature distribution. Specifically, based on the temperature information of the wafer 2 output from the thermocouple thermometer 71 and the temperature information of the wafer 2 calculated from the spectrum output from the detector 97, the control unit 40 adjusts the voltage applied to the electrostatic attraction power supply 31, and controls the mass flow controller 50-4 to adjust the flow rate of He gas, the IR lamp power supply 64, and the chiller 38, thereby maintaining the temperature and temperature distribution of the wafer 2 within a predetermined range.
[0045] (Wafer Processing) Next, referring to FIG. 2, a wafer processing performed in the semiconductor manufacturing apparatus of this embodiment will be described. FIG. 2 is a flow chart showing the wafer processing performed in the semiconductor manufacturing apparatus. Here, a film to be processed in the wafer processing (hereinafter also referred to as a "film to be processed" or "film to be processed") is formed in advance on the wafer 2. The film to be processed is a film containing a typical metal element such as Al2O3, and a process for etching this film will be described. Note that a typical metal element refers to a typical element that does not contain a metalloid element such as Si or a nonmetal element such as C. The process in the flow chart is controlled by the control unit 40.
[0046] <Wafer processing preparation stage> 2, the wafer 2 is transferred by a transfer robot arm or the like. The wafer 2 passes through a wafer transfer port provided in the base chamber 11, is introduced into the processing chamber 1, and is placed on the stage 4.
[0047] The wafer 2 placed on the stage 4 is attracted by an electrostatic attraction mechanism provided inside the stage 4 and fixed onto the stage 4. On the upper surface of the wafer 2, a laminated film structure including a film to be processed, which has been processed into a pattern shape constituting the circuit structure of a semiconductor device, is formed in advance.
[0048] The film to be processed in this embodiment is aluminum oxide (Al2O3), but the technology of this embodiment can also be applied to films of other types of materials. For example, the technology is not limited to films containing typical metal elements such as Al2O3, but can also be applied to films containing transition metal elements. The film structure including the film to be processed is formed to a thickness that can configure a desired circuit using a known sputtering method, PVD (Physical Vapor Deposition) method, ALD (Atomic Layer Deposition) method, CVD (Chemical Vapor Deposition) method, etc. In addition, the film may be processed using photolithography technology to have a shape that conforms to the circuit pattern.
[0049] Furthermore, the control unit 40 adjusts the temperature of the wafer 2. In this embodiment, when it is determined that the temperature of the wafer 2 has reached a first temperature (described in detail later), an etching process for the processing target film of the wafer 2 is started.
[0050] <Wafer Processing in Flowchart> The first step S101 is a step for determining the remaining thickness of the film to be etched formed on the wafer 2. In this step, the control unit 40 determines the remaining thickness of the film to be processed (hereinafter also referred to as the "remaining amount of processing") by appropriately referring to the design and specification values of the semiconductor device to be manufactured using the wafer 2. This step is performed both when etching is performed for the first time after the wafer 2 is carried in and when etching has already been performed on the film to be processed. The calculation unit 41 of the control unit 40 reads out software stored in a storage device arranged inside and performs calculations according to the algorithm described therein. The control unit 40 calculates the value of the cumulative amount of processing (hereinafter also referred to as the "accumulated amount of processing") performed by the processing performed on the wafer 2 before being carried in the processing chamber 1 and the cumulative amount of processing performed by the processing performed after being carried in the processing chamber 1, and determines whether or not additional processing by the technology of the present invention is necessary based on the design and specification values of the semiconductor device to be manufactured using the wafer 2. In this embodiment, the amount of processing is determined for each layer of the physical adsorption layer. The time required for several layers of physical adsorption to cover the sample depends on factors such as the shape of the sample to be processed and the processing stage, so it is desirable to set the time with a safety margin relative to a value determined in advance based on experiments.
[0051] 2 is performed at least once, the accumulated processing amount can be calculated simply from the accumulated number of processing cycles consisting of steps S103 to S109 and the processing amount per processing cycle (cycle processing rate) obtained in advance. The value of the accumulated processing amount calculated in this way is merely a simply estimated value, and therefore may be determined from the output results of a surface analysis of the sample or a film thickness monitoring device (not shown), various process monitoring measurement results such as processed shape and surface roughness, or a combination of these, and it is desirable to combine it with the simply estimated accumulated processing amount from the cycle processing rate and correct or amend it as necessary.
[0052] In step S101, if the remaining amount of processing is determined to be 0, or if a tolerance δ0 that can be regarded as 0 is set and the remaining amount of processing is determined to be smaller than the tolerance δ0, the processing of the film to be processed is terminated. If necessary, for example, RIE using ICP plasma is performed. (Reactive-ion Etching) An etching process using plasma such as etching may be performed.
[0053] If it is determined that the remaining amount of processing is not 0 (or is equal to or greater than δ0), the process proceeds to the next step S102. In step S102, the remaining amount of processing of the film to be processed formed on the wafer 2 is compared with a predetermined threshold value. If it is determined that the remaining amount of processing is greater than the threshold value, the process proceeds to step S103B, and if it is determined that the remaining amount is equal to or less than the threshold value, the process proceeds to step S103A. In the following description, the process from step S103B to step S106B is referred to as process B, Step S The process from step S103A to step S107A is referred to as process A.
[0054] Next, wafer processing performed in the semiconductor manufacturing apparatus 100 of this embodiment will be described with reference to FIGS.
[0055] (Process B) Fig. 3 is a diagram showing a time chart of process B including steps S103B to S106B. Fig. 4 is a diagram showing a time chart of process A including steps S103A to S107A. These figures show the temperature of the wafer 2, and the gas supply and exhaust operations during the etching process of the wafer 2 in this embodiment. The temperatures, temperature gradients, and control times shown in the figures are appropriately selected in consideration of the material to be etched, the type (composition) of the process gas, the structure of the semiconductor device, etc.
[0056] 3, the wafer 2 is electrostatically attracted and He gas is introduced to the rear surface of the wafer 2. In this manner, the temperature of the wafer 2 is maintained at a first temperature T1 as shown in chart 240.
[0057] 2, as shown in a chart 200 of Fig. 3, the supply of the vapor of the chemical solution 44 stored in the tank 45 is started by the mass flow controller 50-5. The vapor of the chemical solution 44 contains a component for converting the processing target film of the wafer 2 placed inside the processing chamber 1 into a volatile organometallic complex, and is an organic gas for the etching process.
[0058] Since this organic gas is a gas for reacting with the film to be treated to form an organometallic complex, for the sake of simplicity, in this disclosure, it may be referred to as a complexing gas hereinafter. In this embodiment, the supply conditions (supply amount, supply pressure, supply time, gas temperature, etc.) of the complexing gas and the type of the complexing gas are determined taking into consideration the elemental composition, shape, and film thickness of the film to be treated in the semiconductor device, and the film configuration in the device. The mass flow controller 50-5 is controlled based on a control signal from the control unit 40.
[0059] In step S103B of FIG. 2, a physisorption layer of complexing gas molecules is formed on the surface of the film to be processed formed on the wafer 2. The control unit 40 determines that a minimum number of physisorption layers are formed in step S103B. This step is performed while maintaining the temperature of the wafer 2 in a temperature range equal to or lower than the boiling point of the complexing gas. As shown in the chart 240 of FIG. 3, the wafer 2 is set to a first temperature T1, and the first temperature T1 is in a temperature range set based on the boiling point of the complexing gas. Note that, as shown in the chart 230, electrostatic adsorption is not performed on the wafer 2, and the supply of He gas is also stopped.
[0060] 2, after a predetermined complexing gas is supplied, the process proceeds to step S104B, where the temperature of the wafer 2 is increased to a second temperature T2. BIn the step, a compound between the film to be treated and the organic gas is formed by heating the wafer 2 while supplying an organic gas containing a substance having at least two substituents with an unshared electron pair in the molecule. In this step, while the supply of the complexing gas is continued, power is supplied from the IR lamp power supply 64 to the IR lamp 62 to emit IR light, and the wafer 2 is irradiated with the IR light. As shown in the chart 220 of FIG. 3, the power of the IR lamp 62 is increased for a predetermined period, then decreased, and then controlled to be kept constant. By this IR light irradiation, as shown in the chart 240, the wafer 2 is heated and quickly raised to the second temperature T2. By heating the wafer 2 to a predetermined second temperature T2 higher than the first temperature T1 and maintaining it at that temperature, a reaction on the surface of the film to be treated is activated, and the adsorption state of the molecules of the complexing gas physically adsorbed on the film surface changes from a physically adsorbed state to a chemically adsorbed state.
[0061] Furthermore, in the next step S105B, the temperature of the wafer 2 is raised to a fourth temperature T4. In this step, the wafer 2 is heated by irradiating IR light emitted from the IR lamp 62 while the supply of the complexing gas into the processing chamber 1 is continued, and as shown in the chart 240 of FIG. 3, the temperature of the wafer 2 is raised to a fourth temperature T4 higher than the second temperature T2. As shown in the chart 220, the power of the IR lamp is increased for a predetermined period of time, then decreased, and then controlled to be kept constant. By this IR light irradiation, as shown in the chart 240, the wafer 2 is heated and quickly raised to the fourth temperature. By raising the temperature to the fourth temperature T4 and maintaining it at that temperature, (1) a first phenomenon in which the organometallic complex generated on the surface of the film to be processed is volatilized and desorbed from the film surface to be removed, and (2) a second phenomenon in which the continuously supplied complexing gas reacts with the surface of the film to be processed to form an organometallic complex proceed in parallel. Regarding step S105B, when a specific small region of the surface of the film to be treated is viewed microscopically, removal of the complexes on the film surface by volatilization (desorption) and formation of new complexes proceed intermittently or stepwise in the order of (1) → (2) → (1) → (2) on the film surface in that region; however, when the surface of the film to be treated is viewed as a whole, it can be considered that etching proceeds essentially continuously.
[0062] Then, the process proceeds to step S106B in FIG. 2, where the supply of the complexing gas is stopped and the inside of the processing chamber 1 is evacuated. In step S106B, based on the result of the comparison in the process of step S102, the wafer 2 is further heated after the process of step S104B to a predetermined temperature, and the organometallic complex is desorbed from the surface of the wafer 2. In step S106B, the wafer 2 is heated while supplying the organic gas, and is continuously heated to the predetermined temperature. As shown in the chart 200 in FIG. 3, the supply of the complexing gas is stopped. While the processes of steps S101 to S105B and S106B are being performed, the pump 15 continues to operate. The processing chamber 1 continues to be evacuated via the vacuum exhaust pipe 16 connecting the pump 15 and the processing chamber 1.
[0063] In step S106B, the supply of the complexing gas is stopped, so that all of the gas containing the organometallic complex volatilized from the film to be treated is exhausted from the treatment chamber 1. At this time, unreacted complexing gas remaining in the piping for supplying the complexing gas, specifically, in the piping from the mass flow controller 50-5 to the treatment chamber 1, is also exhausted by the vacuum exhaust piping 16 and the pump 15 via the treatment chamber 1. Furthermore, exhaust is continued in the steps performed after S106B.
[0064] (Process A) On the other hand, in step S103A of Fig. 2, the supply of the complexing gas is started as shown in chart 200 of Fig. 4. After the control unit 40 forms the minimum number of physical adsorption layers in step S103A, the process proceeds to step S104A, where IR is emitted from the IR lamp 62. Shot The wafer 2 is heated by irradiating it with IR light, and the temperature of the wafer 2 is raised to a second temperature T2, as shown in chart 240 of Fig. 4. As shown in chart 220 of Fig. 4, the power of the IR lamp is controlled to be increased for a predetermined period of time, then decreased, and then kept constant.
[0065] As in step 103B of process B, the supply conditions (supply amount, supply pressure, supply time, temperature) of the complexing gas and the type (composition) of the complexing gas are determined taking into consideration the elemental composition, shape, film thickness, and film configuration of the film to be processed in the semiconductor device. Also, in step S104A, as in step S104B, the temperature of the wafer 2 is raised to a second temperature T2 and then maintained at that temperature, thereby activating the reaction on the surface of the film to be processed, and the adsorption state of the molecules of the complexing gas physically adsorbed on the film surface changes from a physically adsorbed state to a chemically adsorbed state. Step S104 A In the method, an organic gas containing a substance having at least two substituents having an unshared electron pair in a molecule is supplied to a wafer. Add 2 When heated, a compound is formed between the film to be treated and the organic gas.
[0066] The process of step S104A causes the complexing gas to be chemically adsorbed on the surface of the target film, and in this state, the molecules of the complexing gas are firmly fixed by chemical bonds to the metal atoms contained in the target film, for example, Al atoms when the target film is an Al2O3 film. In other words, the molecules of the complexing gas are "pinned" to the surface of the target film.
[0067] As a result, the diffusion rate of the complexing gas molecules from the surface of the membrane to be treated is slow. The diffusion rate of the complexing gas molecules into the interior of the membrane to be treated is particularly slow through the chemisorption layer formed on the surface of the membrane to be treated. The leveling effect caused by the slow diffusion into the interior of the membrane 、S 103A to S107A During the steps up to The surface irregularities of the film to be processed are smoothed. It is considered that the state in which the molecules of the complexing gas are pinned also occurs in step S104B.
[0068] In the next step S105A, the supply of the complexing gas is stopped and the inside of the processing chamber 1 is evacuated. By evacuating the inside of the processing chamber 1, all of the complexing gas that is unadsorbed or physically adsorbed is evacuated from the processing chamber 1, except for the complexing gas that is chemically adsorbed on the surface of the film to be processed. In addition, unreacted complexing gas remaining in the piping for supplying the complexing gas, specifically, the piping from the mass flow controller 50-5 to the processing chamber 1, is also discharged via the processing chamber 1 by the vacuum exhaust piping 16 and the pump 15, and the gas purge mechanism and vacuum mechanism attached to the piping.
[0069] In the next step S106A, the temperature of the wafer 2 is raised to a third temperature T3. In steps S106A and S107A described later, based on the result of the comparison in the step S102, the wafer 2 is further heated after the step S104A to a predetermined temperature, and the organometallic complex is desorbed from the surface of the wafer 2. In steps S106A and S107A, the supply of the organic gas is stopped, and then the wafer 2 is heated in multiple stages to a predetermined temperature. In response to a command signal from the control unit 40, the irradiation intensity of the IR light from the IR lamp 62, which has been continuously irradiated since step S104A, is increased to raise the temperature of the wafer 2 to the third temperature T3. As shown in the chart 220 of FIG. 4, the power of the IR lamp is increased for a predetermined period, then decreased, and then controlled to be kept constant. By this IR light irradiation, the wafer 2 is heated and quickly raised to the third temperature T3, as shown in the chart 240. In this step, the temperature of the wafer 2 is raised to the third temperature T3 and then maintained at that temperature, whereby the molecules of the complexing gas that are chemically adsorbed on the surface of the film to be treated undergo a complexing reaction with the film to be treated on the film surface to form volatile organometallic complexes. Hexo In this step, as shown in chart 200 of FIG. 4, the supply of the complexing gas is stopped. As described above, the complexing gas is not present in the processing chamber 1 except for that which is chemically adsorbed and fixed on the surface of the film to be processed. The amount of the organometallic complex layer produced is determined almost entirely by the amount of the chemically adsorbed layer, and the thickness of the organometallic complex layer is equal to or less than the thickness of the chemically adsorbed layer.
[0070] In the next step S107A, the temperature of the wafer 2 is raised to a fourth temperature T4. The irradiation intensity of the IR light from the IR lamp 62, which continues to be emitted, is further increased to raise the temperature of the wafer 2 to the fourth temperature T4, and the temperature of the wafer 2 is maintained at the fourth temperature T4. As shown in the chart 220 of FIG. 4, the power of the IR lamp is increased for a predetermined period of time, then decreased, and then controlled to be kept constant. By this IR light irradiation, as shown in the chart 240, the wafer 2 is heated and quickly raised to the fourth temperature T4. In this process, the temperature at which the organometallic complex formed in the previous step S106A volatilizes and desorbs is maintained, and the organometallic complex is removed from the surface of the film to be treated.
[0071] (Actions of Process A and Process B) Process A, which is composed of a series of steps S103A → S104A → S105A → S106A → S107A, and process B, which is composed of a series of steps S103B → S104B → S105B → S106B, are the same in that the wafer 2 is heated to a second temperature T2 to form a chemisorption layer on the surface of a film containing a transition metal. However, the two processes are different from each other in the step after the step in which the chemisorption layer is converted into an organometallic complex.
[0072] That is, as shown in step A, when the temperature of the organometallic complex or the film having the organometallic complex on its surface is raised to a fourth temperature T4 at which the organometallic complex is volatilized and removed while the supply of the complexing gas is stopped, the volatilization and removal of one to several layers of the organometallic complex converted from the chemical adsorption layer is completed, and the reaction is terminated when the film to be treated directly below is exposed in the treatment chamber 1. On the other hand, as shown in step B, when the temperature is raised to a fourth temperature T4 at which the organometallic complex is volatilized and removed while the supply of the complexing gas is continued, the volatilization and removal of one to several layers of the organometallic complex converted from the chemical adsorption layer is completed, and the unreacted film to be treated directly below is exposed, the exposed film to be treated is heated to the fourth temperature T4 and its reactivity is increased, so that it is directly converted to the organometallic complex by contact with the complexing gas. Furthermore, the generated organometallic complex is quickly volatilized and removed, and etching of the film to be treated proceeds continuously as a whole.
[0073] In step B, the film to be treated is directly converted to an organometallic complex, which is then volatilized and removed, and therefore the chemically highly active micro-regions present on the surface of the film to be treated, such as grain boundaries and specific crystal orientations, are preferentially converted to organometallic complexes and removed. In addition, when a chemical adsorption layer is formed, a self-organized planar orientation growth process occurs, but in step B, the organometallic complex layer is formed directly without going through this self-organized planar orientation growth process, so the organometallic complex layer has almost no orientation. As a result, the surface of the film to be treated after treatment is not flattened, but rather the unevenness increases and the surface becomes rough.
[0074] On the other hand, in process A, the surface of the film to be treated, for example an Al2O3 film, becomes increasingly flattened due to the effect of self-organized orientation when the chemical adsorption layer is formed and the effect of suppressing the diffusion rate of complexing gas molecules within the chemical adsorption layer that has grown with an orientation in a self-organized manner.
[0075] The fourth temperature T4 is set after a prior evaluation prior to processing of the wafer 2 so as to be lower than the decomposition start temperature of the complexing gas molecules and the decomposition start temperature of the organometallic complex molecules and higher than the volatilization start temperature of the organometallic complex molecules. If the temperature difference between the decomposition start temperature and the volatilization start temperature of the organometallic complex molecules is small and insufficient in consideration of the specifications of the semiconductor manufacturing apparatus 100, for example, the characteristics of the uniformity of temperature in the surface direction of the upper surface of the stage 4, then an existing method for lowering the volatilization start temperature of the organometallic complex molecules, for example, mean free line In order to extend the range, a method such as reducing the pressure inside the processing chamber 1 may be applied.
[0076] If the decomposition start temperature of the organometallic complex molecule is found to be lower than the volatilization start temperature by the preliminary evaluation, the combination of the material of the film to be processed and the organic gas molecule for etching is inappropriate, so another substance is selected from the candidate materials for the organic gas for etching described below. Note that by actively utilizing the inconsistency in the combination of the material of the film to be processed and the organic gas molecule for etching, it is possible to selectively etch only a layer of a specific material in the multilayer film structure.
[0077] (Steps after Process A and Process B) Next, a common step performed after step A and step B will be described. The process proceeds to step S108, and cooling of the wafer 2 is started. As shown in the chart 220 of FIG. 3 and FIG. 4, the power supply to the IR lamp is stopped, but a process of exhausting the complexation gas without fail is performed before the start of S108. As shown in the chart 200 of FIG. 3 and FIG. 4, the supply of the complexation gas has already been stopped before the start of S108, and the unreacted complexation gas remaining and staying in the piping for supplying the complexation gas, specifically, the piping from the mass flow controller 50-5 to the processing chamber 1, should have already been exhausted. However, if the unreacted complexation gas remains somewhere due to some kind of trouble or unexpected event, there is a risk that it may cause the generation of foreign matter, so in this embodiment, an operation of exhausting the unreacted complexation gas via the processing chamber 1 by the vacuum exhaust piping 16 and the pump 15 is performed again.
[0078] In addition, it is adsorbed to the inner wall of the pipe. storage In order to remove the complexing gas remaining in the piping, a so-called purging operation is performed before proceeding to the cooling step S108, in which the inside of the piping from the mass flow controller 50-5 to the processing chamber 1 is filled with an inert gas and then exhausted. In order to reliably exhaust the gas remaining or stagnating in the piping from the mass flow controllers 50-1, 50-2, 50-3, 50-4, 50-5 to the processing chamber 1, a waste gas path (not shown) may be provided as necessary.
[0079] In both the flows of steps A and B, the process proceeds to step S108, where cooling of the wafer 2 is started, and continues until it is detected in step S109 that the temperature of the wafer 2 has reached a predetermined first temperature. As shown in the chart 230 in FIG. 3 and FIG. 4, the wafer 2 is electrostatically attracted and He gas is supplied to the back surface of the wafer 2. In the substrate cooling step S108, it is desirable to supply a cooling gas between the stage 4 and the wafer 2. For example, He or Ar is suitable as the cooling gas, and supplying He gas can cool the wafer in a short time, thereby increasing processing productivity. As described above, the stage 4 is provided with a flow path 39 connected to the chiller 38 inside, so that the wafer 2 is gradually cooled even when it is merely electrostatically attracted to the stage 4 and no cooling gas such as He is flowing.
[0080] As described above, thermocouples 70 for measuring the temperature of stage 4 and optical fibers 92 for detecting the wafer temperature are arranged at multiple locations inside stage 4, and are connected to corresponding thermocouple thermometers 71 and detectors 97, respectively. Any means for appropriately measuring the temperatures of wafer 2 and wafer stage 4 can be used as the temperature measuring means. When controller 40 detects, based on signals obtained by these temperature measuring means, that stage 4 has reached a predetermined temperature, for example, first temperature T1 as shown in charts 240 in Figs. 3 and 4, one cycle of the process of etching the target film on wafer 2 is completed.
[0081] After the control unit 40 determines that the temperature of the wafer 2 has reached the first temperature T1 and the first cycle process is completed, the process returns to step S101 to determine whether the remaining processing amount has reached 0. As described above, when the control unit 40 determines that the remaining processing amount has reached 0, the etching process of the processing target film of the wafer 2 is terminated, and when it is determined that the remaining processing amount is greater than 0, the process proceeds again to step S102 to perform the process of either step A or step B.
[0082] Specifically, the result of the judgment is "machining residue" amount If the result of the determination in S102 is "large", the processes in steps S103B to S106B, S108, and S109 are carried out in that order, as described above. amount If the result is "small," the processes are carried out in the order of steps S103A to S107A, S108, and S109.
[0083] When the processing of the wafer 2 is finished, the supply of the cooling He gas is stopped. Furthermore, a step of discharging the He gas from the back surface of the wafer 2 by opening the valve 52 arranged on the waste gas path connecting the He gas supply path and the vacuum exhaust pipe 16 from closed, and a step of releasing the electrostatic adsorption of the wafer 2 are also performed.
[0084] Thereafter, the processed wafer 2 is delivered to the transfer robot through the wafer transfer port of the base chamber 11, and the next unprocessed wafer 2 to be processed is transferred in. Of course, if there is no next unprocessed wafer 2 to be processed, the wafer transfer gate is closed and the operation of manufacturing semiconductor devices by the semiconductor manufacturing apparatus 100 is stopped.
[0085] In this embodiment, the second temperature T2, the third temperature T3, and the fourth temperature T4 set in each of the above-mentioned processes A and B do not necessarily have to be the same between processes A and B. Appropriate temperature ranges can be set through careful consideration before processing the wafer 2. The control unit 40 sets the temperatures for each step in processes A and B according to the specifications of the film to be processed on the wafer 2.
[0086] [Example 1] Next, a semiconductor manufacturing method carried out in the semiconductor manufacturing apparatus of this embodiment will be described with reference to a specific example.
[0087] In this embodiment, before starting the etching process of the wafer 2, the wafer 2 is transported and held by adsorption on the stage 4 in the process chamber 1. A film to be processed containing a typical metal element and processed into a desired pattern shape, for example, an Al2O3 film surface, is formed in advance on the surface of the wafer 2, and a part of it is exposed.
[0088] After the wafer 2 is electrostatically attracted and held on the stage 4, the pressure inside the processing chamber 1 is reduced and the wafer 2 is heated. As the wafer 2 is heated and its temperature is increased, gas (such as water vapor) and foreign matter that are attracted to the surface of the wafer 2 are desorbed.
[0089] When it is confirmed that the gas components adsorbed on the surface of the wafer 2 have been sufficiently desorbed, the heating of the wafer 2 is stopped and cooling of the wafer 2 is started while maintaining the reduced pressure inside the processing chamber 1. In this process, known means can be used for heating and cooling, and for example, heat conduction from a heater arranged inside the stage 4 or radiation of light emitted from a lamp is used for heating.
[0090] In addition to these heating methods, foreign matter adhering to the wafer 2 may be removed by, for example, ashing or cleaning the surface using plasma generated in the processing chamber 1. Note that this wafer heating step may be omitted when it is known for certain that the surface of the wafer 2 is sufficiently clean and free of adsorbed or attached matter, but it is desirable to carry out this step from the viewpoint of warming up the processing chamber 1, particularly the inner wall of the processing chamber 1.
[0091] When the control unit 40 determines that the temperature of the wafer 2 has dropped and reached a predetermined first temperature T1 or a temperature lower than this, the wafer 2 is processed according to the flow chart shown in Fig. 2. Note that before the wafer 2 starts to be processed, for example before it is loaded into the processing chamber 1, the control unit 40 detects the processing conditions, such as the type and flow rate of gas used to process the film to be processed on the wafer 2, the pressure inside the processing chamber 1, and the like, that is, the processing recipe. For example, the ID of each wafer 2 is obtained by reading the markings on the wafer 2, or the like. (Identification) The number is acquired, and data of the wafer 2 corresponding to the ID number is acquired by referring to data from a production management database via a communication facility such as a network connected to the control unit 40. The data includes the processing history, the composition, thickness, and shape of the target film to be etched, the amount of etching of the target film (target remaining film thickness, etching depth), and the etching end point conditions.
[0092] For example, assume that the control unit 40 detects that the process to be performed on the wafer 2 is an etching process to remove an Al2O3 film of 0.2 nm, which is smaller than a predetermined threshold (e.g., 0.5 nm). In this case, since the ionic radii of aluminum (3+) and oxygen (2-) are about 0.5 angstroms and about 1.3 angstroms, respectively, it is determined that the process is a process to remove about one atomic or molecular layer of Al2O3, and it is determined that "remaining amount of processing ≦ threshold" in step S102 of FIG. 2. Then, according to the flow of process A (S103A → S104A → S105A → S106A → S107A), the control unit 40 transmits a signal to each unit of the semiconductor manufacturing equipment 100 to perform film processing. Note that the amount of etching of the processing target film for each cycle of process A is measured in advance, and the above-mentioned predetermined threshold is set based on the measured value of the cycle processing amount of process A.
[0093] On the other hand, when the control unit 40 judges that the process is to remove an Al2O3 film 5 nm thick that exceeds a predetermined threshold (e.g., 0.5 nm), 10 or more layers, nearly 20 layers, must be removed. If the above-mentioned layer-by-layer etching is performed, the process will be repeated 10 times or more, and the process time will increase by n times, resulting in a loss of productivity. Therefore, first, multiple layers (e.g., 7 to 8 layers or more) are removed together, and then the remaining film layers are removed one by one. In this embodiment, in such a case, the film to be processed is processed at least once according to the flow of process B (S103B → S104B → S105B → S106B) which is shifted to after it is judged that "processing remaining amount>threshold" in FIG. 2, and then the flow of process A (S103A → S104A → S105A → S106A → S107A) is performed, and the Al2O3 film 5 nm thick is removed by the total flow of process B and process A. The amount of the film to be processed etched each time step B is performed in one cycle is measured in advance, and the number of times step B is repeated is set based on the measured value of the cycle processing amount of step B and the amount of removal by etching.
[0094] The first step S103A of process A and the first step S103B of process B shown in FIG. 2 are processes for forming a physically adsorbed layer of the complexing gas on the surface of the film to be processed, and are performed by maintaining the temperature of the wafer 2 at a temperature equal to or lower than the boiling point of the complexing gas. For example, when the boiling point of the complexing gas is about 300° C., Ha2 It is common to set the temperature at about 250°C to 280°C, or up to a maximum temperature of about 300°C.
[0095] For example, 2-cyanophenol is an organic substance with a boiling point of about 300°C, and is suitable for the complexing gas. When 2-cyanophenol is used, the first temperature T1 is preferably in the range of about 200°C to 280°C, more preferably in the range of 220°C to 270°C. If the first temperature T1 is below 200°C, it takes time to raise and lower the temperature at the stage of moving to the next steps S104A and S104B, and there is a risk that the productivity will be reduced. Conversely, if the first temperature T1 is above 280°C, the adsorption efficiency (adhesion characteristics) of 2-cyanophenol will decrease, and the gas flow rate of 2-cyanophenol will have to be increased in order to adsorb a predetermined amount in a short time, which may increase gas consumption and increase operating costs.
[0096] In this way, after the physical adsorption layer is formed in step S103A or S103B, the wafer 2 is heated by the IR light emitted from the IR lamp 62 in steps S104A and S104B, and is quickly heated to the second temperature. This changes the adsorption state of the complexing gas on the surface of the film to be processed from a physical adsorption state to a chemical adsorption state. The temperature increase in this step is for providing activation energy to cause a change in the adsorption state of the molecules of the complexing gas adsorbed on the surface of the film to be processed.
[0097] The second temperature is determined in consideration of the influence of both the surface state of the film to be treated and the characteristics (reactivity) of the complexing gas. For example, when a complexing gas mainly composed of 2-cyanophenol is supplied to an Al2O3 film as the film to be treated, the second temperature is in the range of about 220°C to 310°C, and appropriate conditions are determined within that range by comprehensively considering the state of the film to be treated and the balance with the third temperature described later. In the case of a complexing gas mainly composed of 2-cyanophenol, if the temperature is lower than 220°C, it takes a long time to convert to a chemical adsorption layer, and if the temperature exceeds 310°C, it will not remain in a chemical adsorption state but will be converted to an organometallic complex. In addition, when supplied under reduced pressure, the temperature exceeds the temperature at which the organometallic complex begins to volatilize as described later, so there is a risk of the controllability of the film thickness being reduced.
[0098] Next, in the case of step B, while maintaining the supply of the complexing gas, infrared heating using the IR lamps 62 is continued and the power supplied to the IR lamps 62 is increased to raise the temperature to a fourth temperature (step S105B). The fourth temperature is set to a temperature lower than the temperature at which thermal decomposition of the volatile organometallic complex generated by the reaction between the surface material of the film to be treated and the complexing gas occurs, and equal to or higher than the temperature at which sublimation or volatilization begins.
[0099] In step S105B, after the temperature of the wafer 2 is set to the fourth temperature, the temperature of the wafer 2 is maintained at the fourth temperature T4 at least until the supply of the complexing gas is stopped in step S106B. By such a flow, the surface of the film to be processed is substantially continuously etched in process B.
[0100] On the other hand, in the case of process A, the supply of the complexing gas such as 2-cyanophenol is stopped as shown in step S105A, the inside of the processing chamber 1 is evacuated, and then the wafer 2 is heated to a third temperature using the IR lamps 62 as shown in step S106A. By maintaining the temperature of the Al2O3 film at the third temperature for a predetermined period of time, the chemical adsorption layer formed on the surface of the Al2O3 film is converted into an organometallic complex.
[0101] The third temperature is set to a value within an appropriate range that is equal to or higher than the second temperature and lower than the volatilization start temperature of the organometallic complex molecules, taking into consideration the stability of temperature control in the semiconductor manufacturing equipment 100 and the control unit 40, and the accuracy of temperature measurement of the wafer 2 and the wafer stage 4 by the thermocouple thermometer 71 or an alternative temperature measurement means. In the case of an etching process using an Al2O3 film as the processing target film and a mixed gas containing 2-cyanophenol as the complexing gas as the main component, according to an experiment by the inventor, the volatilization start temperature of the organometallic complex molecules was found to be around 270°C under reduced pressure conditions, so that the appropriate maximum temperature for the third temperature is around 250°C.
[0102] After the wafer 2 is maintained at the third temperature set in step S106A for a predetermined period of time, the intensity of the IR light emitted from the IR lamps 62 is increased slightly to raise the temperature of the wafer 2 to a fourth temperature in step S107A. By maintaining the wafer 2 at the fourth temperature T4, the organometallic complex converted from the chemical adsorption layer is volatilized and removed. At the start of step S107A, only one to several layers, or at most five layers, of the organometallic complex have been generated, so that they are quickly volatilized and removed after the fourth temperature is reached.
[0103] When the organometallic complex is volatilized and removed, the reaction for one cycle ends when the film to be treated or a layer of a silicon compound or the like disposed under the film to be treated is exposed. In the case of a treatment using, for example, an Al2O3 film as the film to be treated and a mixed gas containing 2-cyanophenol as the complexing gas, the preferable range of the fourth temperature is generally in the range of 270°C to 400°C. If the temperature is lower than 270°C, the sublimation and volatilization speed is slow, and the efficiency of the treatment is impaired. Conversely, if the temperature exceeds 400°C, part of the organometallic complex may be thermally decomposed during the process of sublimation and volatilization, and may become a foreign matter, which may adhere to the surface of the wafer 2 or the inside of the treatment chamber 1.
[0104] [Variation 1] Next, a modified example of the etching process will be described with reference to Fig. 5. In that the temperature of the wafer is raised to the second temperature and a complexing gas is supplied at the same time, ,fruit The embodiment differs from the first embodiment. Fruit Components that are the same as or equivalent to those in the embodiment and the first embodiment are given the same reference numerals, and their description will be simplified or omitted.
[0105] FIG. 5 is a diagram showing a time chart of a modified example performed in a semiconductor manufacturing apparatus.
[0106] 2, steps S101 and S102 are performed to detect the amount of remaining etching processing and compare the amount with a threshold value. Next, after the control unit 40 determines that the temperature of the wafer 2 is equal to or lower than a first temperature, step S103C is performed. In step S103C, a complexing gas is supplied into the processing chamber 1 as shown in chart 200, and a process is started in which molecules of the complexing gas are adsorbed on the surface of the film to be processed to form a physical adsorption layer.
[0107] Immediately after the start of step S103C, as shown in chart 220, power is supplied to the IR lamp 62 to emit infrared rays, which heats the wafer 2 and quickly raises the temperature of the wafer 2 to the second temperature T2, as shown in chart 240. As shown in chart 240, the supply of the complexing gas to the process chamber 1 is continued while maintaining the temperature of the wafer 2 at the second temperature for a predetermined period of time. Therefore, during the period of step S103C, a reaction for forming a physisorption layer of the complexing gas component on the surface of the film to be treated and a conversion reaction for converting the physisorption layer to a chemisorption layer proceed continuously in parallel.
[0108] In this case, as described above, the diffusion rate of the complexing gas molecules into the inside of the film to be treated through the chemical adsorption layer formed on the surface of the film to be treated is slow, so that the thickness of the chemical adsorption layer saturates with the treatment time. After the film thickness of the chemical adsorption layer is saturated by continuing the supply of the complexing gas for a predetermined time while maintaining the temperature at approximately the second temperature T2, the supply of the complexing gas is stopped in the next step S105C as shown in chart 200.
[0109] 5, before step S103C of supplying the complexing gas is performed, in other words, from the time when the temperature of the wafer 2 is equal to or lower than the first temperature T1 specified in advance, the pump 15 is driven to maintain the internal pressure of the processing chamber 1 at a reduced pressure as shown in the chart 250. Therefore, when the supply of the complexing gas is stopped in step S105C, all of the complexing gas that is not adsorbed or is physically adsorbed is exhausted and removed to the outside of the processing chamber 1, except for the complexing gas that is chemically adsorbed to the surface. In order to promote the exhaust and removal of the organic etching gas physically adsorbed to the inner wall of the processing chamber 1 to the outside of the processing chamber 1, it is preferable to continue to supply a small amount of Ar gas to the inside of the processing chamber 1 as shown in the chart 260.
[0110] The supply amount of Ar gas and the pressure in the processing chamber 1 need to be adjusted appropriately depending on the film to be processed and the composition of the complexing gas, but when etching an Al2O3 film using a complexing gas mainly composed of 2-cyanophenol, the Ar supply amount is preferably 200 sccm or less and the processing chamber pressure is preferably about 0.5 to 3.0 Torr. Furthermore, the preferred Ar supply amount is about 100 sccm and the processing chamber pressure is about 1.5 Torr.
[0111] If the Ar supply rate exceeds 200 sccm, the effective concentration of the complexing gas in the processing chamber 1 decreases, decreasing the efficiency of adsorption to the surface of the film to be processed, and increasing the risk of causing a decrease in the etching rate. On the other hand, if the pressure in the processing chamber falls below 0.5 Torr, the residence time of the complexing gas in the processing chamber 1 becomes shorter, increasing the risk of causing a decrease in the efficiency of use of the complexing gas. In order to adjust the pressure in the processing chamber to exceed 3 Torr, the Ar supply rate must be set to 200 sccm or more, decreasing the efficiency of adsorption of the complexing gas to the surface of the film to be processed, and increasing the risk of causing a decrease in the etching rate.
[0112] Next, the temperature of the wafer 2 is raised to a fourth temperature T4 as shown in chart 240 by infrared heating using the IR lamps 62 as shown in chart 220. In step S106C, the temperature of the wafer 2 is maintained at approximately the fourth temperature T4 for a predetermined time. During the process of raising the temperature to the fourth temperature T4 and maintaining the temperature, the chemical adsorption layer is converted into an organometallic complex and the corresponding Yes The volatilization and removal of the organometallic complex proceeds. When an Al2O3 film is used as the film to be processed and a gas containing 2-cyanophenol as the main component is used as the complexing gas, the suitable range of the fourth temperature T4 is 270°C to 400°C. If the temperature is lower than 270°C, sublimation or volatilization is slow and a practical etching rate cannot be obtained, and conversely, if the temperature exceeds 400°C, part of the organometallic complex will thermally decompose at a location below 400°C in the process of sublimation and volatilization of the organometallic complex, and there is a high possibility that the organometallic complex will be redeposited on the surface of the wafer 2 or inside the processing chamber 1 as a foreign matter.
[0113] When the film to be treated or a layer of a silicon compound or the like disposed under the film to be treated is exposed, the process of volatilizing and removing the organometallic complex is completed. After that, when the infrared heating using the IR lamp 62 is stopped as shown in chart 220, the temperature starts to decrease due to heat radiation from the wafer 2 as shown in chart 240. When the temperature of the semiconductor wafer 2 reaches the second temperature T2 or a temperature lower than that, one cycle of processing is completed.
[0114] Thereafter, the second and subsequent cycle processes starting from step S103C through step S102 are repeated a desired number of times to achieve etching to a desired thickness. The modified example shown in Fig. 5 is a simplified version of the example shown in Fig. 4, in which the number of temperatures set is reduced and the temperature range of the cooling step in S108, which takes particularly long, is narrowed to shorten the time per cycle.
[0115] [Variation 2] Next, still another example of the above-mentioned etching process for the wafer 2 will be described.
[0116] In this example, a first processing target film, e.g., an Al2O3 film, containing a typical metal element processed into a desired pattern shape, as well as a second processing target film, e.g., an HfO2 film, containing a transition metal element below the fifth period of the periodic table, are formed in advance on the surface of the wafer 2 used in this example, and a part of them is exposed. In this example, in order to selectively etch the Al2O3 film as the first processing target film and the HfO2 film as the second processing target film, respectively, a first etching gas for etching only the first processing target film and a second etching gas for etching only the second processing target film are used separately.
[0117] As will be explained in more detail below, the film configuration described here (such as the film thickness ratio of the first film to be processed and the second film to be processed) is merely an example, and the film thickness can be adjusted to the required thickness depending on the application and purpose. A 2.0 nm thick Al2O3 film as the first film to be processed and a 5.0 nm thick HfO2 film as the second film to be processed are alternately stacked to form a layered structure of Al2O3-HfO2-Al2O3, and a patterned resist is placed on the top layer Al2O3 film. The top layer Al2O3 film is formed on the surface of the wafer 2 with a part of the Al2O3 film exposed from the opening of the resist pattern.
[0118] The wafer 2 having such a laminated film structure including the film to be processed is FruitAs in the embodiment and Example 1, the wafer is introduced into the processing chamber 1 and adsorbed and fixed on the wafer stage 4, and the amount of etching to be performed on the layer to be processed is determined, and step A or step B is selected according to the thickness to be processed, and the selected step is performed. At this time, when selectively etching only the Al2O3 layer or only the HfO2 layer of the laminated film in which different materials are laminated, a processing step using an etching material that etches only the 2.0 nm thick Al2O3 film and a step using an etching material that etches only the 5.0 nm thick HfO2 film are sequentially performed.
[0119] Below, an example of a process flow in which only a 2.0 nm thick Al2O3 film is etched, followed by a 5.0 nm thick HfO2 film is etched in that order. The Al2O3 film to be etched first is 2.0 nm thick, and since the remaining film thickness is sufficiently large, multiple layers are etched and removed continuously, rather than being etched one atomic layer at a time. In other words, the process of step B in Figure 2 is selected, and the etching process is started from the step of supplying a first complexing gas suitable for etching the Al2O3 film in step S103B.
[0120] In this modification, the first complexing gas may be, for example, 2-cyanophenol. The complexing gas containing 2-cyanophenol as a main active ingredient is supplied to the processing chamber 1 by a mass flow controller 50-5-1 (not shown). At this time, since 2-cyanophenol has a small vapor pressure at 100° C. or less under normal pressure, it is desirable to heat the supply pipe and reduce the pressure inside the pipe to about 2 kPa or less. If necessary, the complexing gas can be efficiently supplied by combining it with a vaporization promotion means other than pressure reduction and heating, such as ultrasonic atomization, or atomization of a solution obtained by dissolving the gas in an appropriate solvent.
[0121] In step S103B, 2-cyanophenol is adsorbed on the top surface of the Al2O3 film to form an adsorption layer. By sequentially processing S104B, S105B, and S106B, the adsorption layer of Al2O3 and 2-cyanophenol is formed. This was obtained by the reaction ofAfter the organic Al complex layer is generated, it is removed by volatilization. After that, the process of step B and the process of step A are carried out the number of times required to remove the 2.0 nm thick Al2O3 film, and when the Al2O3 film is removed, the 5.0 nm thick HfO2 film underneath is exposed.
[0122] Since the HfO2 film does not react with 2-cyanophenol, it is possible to completely remove the Al2O3 film on the HfO2 film by repeating only the process of step B. However, if the Al2O3 film is removed only by the process of step B, side etching may occur at the bottom of the resist opening, and the desired pattern shape and pattern dimensions may not be obtained. Therefore, in this example, it is preferable that the timing at which the process of step B is completed and the process of step A is switched to be based on whether or not at least a part of the Al2O3 film has been removed and a part of the HfO2 film underneath is exposed, rather than on the remaining film thickness. However, in this example, when the lower HfO2 film is partially exposed, it can be said that the remaining film thickness of the upper Al2O3 film is also sufficiently small. Therefore, the remaining Al2O3 film thickness at the time when the HfO2 film is partially exposed can be used as the threshold value in step S102 of FIG. 2.
[0123] Next, selective etching of the HfO2 film is performed. The second complexing gas is, for example, HF and TiCl4, as described in Non-Patent Document 1. The HfO2 film can be etched by repeating a process consisting of four steps: HF gas is supplied from a mass flow controller 50-5-2 (not shown) for 1 second, nitrogen is supplied as a purge gas for 30 seconds, and then nitrogen is supplied as a purge gas for 2 seconds from a TiCl4 mass flow controller 50-5-3 (not shown) for 30 seconds.
[0124] Under these processing conditions, the Al2O3 film is not etched, but the HfO2 film is selectively and conformally etched, so that the HfO2 film is etched in a shape that follows the etched shape of the Al2O3 film. Since the etched shape of the Al2O3 film is processed according to the opening pattern shape of the top layer resist film, the shape is also transferred to the HfO2 film. After about 250 repeated processes, the desired shape of the 5.0 nm thick HfO2 film is removed, exposing the 2.0 nm thick Al2O3 film underneath the HfO2 film.
[0125] In this way, the technology of the present invention can be combined with known techniques appropriately to realize highly accurate selective processing of multilayer structures. In this embodiment, it has been specifically described that Al2O3-HfO2 of a desired shape can be selectively removed from the upper layer side of a laminated film of Al2O3-HfO2-Al2O3. In the case of a combination of film materials other than those exemplified here and a film thickness to be removed, etching is possible even for many types of laminated films by appropriately selecting an appropriate complexing gas in advance and combining it with known techniques as necessary. However, as mentioned above, it is necessary to note that there are practical limitations to the fact that known techniques use a combination of many types of etching gases to etch one layer.
[0126] [Complex gas components] Next, the components of the complexing gas suitable for the present invention will be described with reference to Fig. 6. Fig. 6 is a diagram showing the molecular structures of the components of the complexing gas.
[0127] The main active ingredient of a complexing gas is a substance that has two or more atoms (electron-donor atoms) with unshared electron pairs that exhibit an electric charge interaction, specifically an electron-donating effect, with the positive charges of the metal atoms contained in the film to be etched, and that has a molecular structure in which the electron-donor atoms are not directly bonded to each other and there is at least one carbon atom between the electron-donor atoms (e.g., OCO, rather than OO, etc.).
[0128] In addition, if it has π electrons that have an electron-donating effect on the positive charge of the metal atom contained in the metal film, it may function as a substitute for an atom with an unshared electron pair. For example, the electron pair on the nitrogen atom of the indole ring is incorporated into the π conjugation of the entire indole ring, but the indole ring as a whole has an electron-donating effect on the positive charge of the metal atom. If the molecule of the etching gas active ingredient has a molecular structure that has an electron-donating effect on the positive charge of the metal atom at two or more places, it forms a strong electron-donating and reverse-donating coordinate bond by donating electrons to the positive charge of the metal element of the etched film, forming a thermally stable complex compound.
[0129] Specific examples of substances having such molecular structures include substances having the characteristics of the following molecular structure formulas (1) to (3). A liquid containing at least one substance having such a molecular structure and, if necessary, dissolving it in an appropriate diluent is used as chemical solution 44, which is the raw material for the complex gas. By using a liquid dissolved in an appropriate diluent, the diluent promotes vaporization of the active ingredient of the complex gas, and further, the vaporized diluent functions as a carrier gas, enabling smooth supply.
[0130] (Molecular structural formula (1)) The molecular structure illustrated in Figure 6(1) has a phenol skeleton in which an OH group having an unshared electron pair is bonded to a benzene ring. As viewed from the carbon atom to which the OH group is bonded, the phenol skeleton has one substituent selected from an OH group, an OCH3 group, an OCOCH3 group, an OCONH2 group, an NH2 group, an N(CH3)2 group, etc., which is an electron-donating substituent at the adjacent position Y (ortho position) from the carbon atom to which the OH group is bonded. In addition, any one of halogen atoms (F, Cl, Br, I) may be bonded to the diagonal position X (para position) of the benzene ring from the carbon atom to which the OH group is bonded.
[0131] (Molecular structure formula (2)) The molecular structure illustrated in Figure 6(2) has a phenol skeleton in which an OH group, which is a partial structure having an unshared electron pair that exhibits electron-donating properties, is bonded to a benzene ring. The adjacent position X1 (ortho position) from the carbon atom to which the OH group is bonded has one substituent selected from a CN group, a CH=CH-CH3 group, a CH=CH-CN group, a CH=CH-CO2CH3 group, etc. The diagonal position X3 (para position) of the benzene ring from the carbon atom to which the OH group is bonded may have one substituent selected from a CH=O group, a CN group, a NO2 group, etc.
[0132] When the ortho position has a CN group, it is called a 2-cyanophenol, and when the ortho position has a CH=CH-CO2CH3 group, it is called an o-hydroxycinnamic acid ester, and the unsaturated bond of the CN group or CH=CH-CO2CH3 group has a π electron that functions as an electron donor instead of an atom with an unshared electron pair. In addition, the induced electron withdrawing action of the CN group or CH=CH-CO2CH3 group increases the reactivity of the OH group.
[0133] Positions X2 and X4 have H. Position X5 has one substituent selected from H, CH=O group, CN group, NO2 group, SOCH3 group, CH=CH-CH3 group, CH=CH-CN group, CH=CH-CO2CH3 group, etc.
[0134] (Molecular structure formula (3)) The molecular structure illustrated in Figure 6(3) is an aliphatic 4-membered ring compound having a carbonyl group, and the carbonyl group is bonded to an O atom, which is a partial structure having an unshared electron pair. This structure is a substance that has two atoms (electron-donating atoms) having an unshared electron pair that exhibits electron-donating action, the O of the carbonyl group protruding outside the 4-membered ring and the O that forms the 4-membered ring, and at least one carbon atom is located between the electron-donating atoms. As a specific example, β-butyrolactone is a substance in which position R1 is a methyl group.
[0135] The molecular structures shown in Figures 6(1) and (2) have atoms or substituents that exhibit electron-donating properties in at least two places, and they exhibit electrostatic interactions with the positive charges of the metal atoms in the film to be etched, resulting in efficient adsorption. When heated in the adsorbed state, two coordinate bonds are formed between the atoms that exhibit electron-donating properties and the metal atoms in the film to be etched so that the charges of each other are cancelled out, forming an organometallic complex.
[0136] As mentioned above, this coordinate bond is a strong bond of electron donor and reverse donor type, and since the bond is formed at two places, it is a thermally stable complex compound. Metal acetates and metal formates obtained by the reaction of simple acetic acid or simple formic acid with typical metals have only one bond, so their stability is not necessarily high. In contrast, the intermediate organometallic complexes formed by the technology of the present invention have significantly improved thermal stability compared to these carboxylates, and as a result, they are easily volatilized and removed.
[0137] The molecular structure illustrated in Fig. 6(3) has a smaller molecular cross-sectional area than the molecular structures illustrated in Fig. 6(1) and (2), and therefore has the property of being easily volatilized at low temperatures, and can be efficiently vaporized even with a vaporization supply 47 having a relatively simple structure. When a substance having this molecular structure is adsorbed onto the surface of the film to be etched, the aliphatic four-membered ring is opened by electrostatic interaction with the positive charges held by the metal atoms contained in the film to be etched, and then the substance is converted into an organometallic complex having a five- or six-membered ring structure in which the metal element is incorporated into the ring. The resulting cyclic organometallic complex is a thermally stable complex compound, and as a result, it is easily volatilized and removed.
[0138] [Actions and Effects] In this embodiment, the processing gas used for etching is one type of organic gas. Therefore, a semiconductor device can be manufactured without requiring a complicated gas supply system. In addition, since gas replacement is not required, the etching efficiency is not reduced. In addition, since the compound has a property of being highly thermally stable, it does not become a foreign matter during exhaust. Therefore, according to the present embodiment, a manufacturing method for a semiconductor device is possible that does not require a complicated gas supply system, ensures processing efficiency, and suppresses the generation of foreign matter. and A semiconductor manufacturing device can be provided.
[0139] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-described embodiment, and various modifications are possible without departing from the gist of the present invention. [Explanation of symbols]
[0140] 1. Treatment chamber, 2. Semiconductor wafer, 3...discharge area, 4. Wafer stage, 5. Shower plate, 6. Top plate, 11... Base chamber, 12...Quartz chamber, 14... Pressure adjusting mechanism, 15 Pump, 16 Vacuum exhaust piping, 17 Gas distribution plate, 20...High frequency power supply, 22...matching box, 30: Electrostatic adsorption electrode, 31... Electrostatic adsorption power supply, 34...ICP coil, 38 Chiller, 39... flow path, 40... Control unit, 41...Arithmetic section, 45···Tank, 46 Heater, 47 Vaporizer, 50-1~50-5 Mass flow controller, 51: Integrated mass flow controller control section; 52, 53, 54... valve, 60...container, 62...IR lamp, 63...reflector, 64···Power supply for IR lamp, 70...thermocouple, 71 Thermocouple thermometer, 74...IR light transmitting window, 75 Gas flow path, 78...Slit plate, 81... O-ring, 92 Optical fiber, 93...external IR light source, 94... Optical path switch, 95...optical distributor, 96...Spectrometer, 97... Detector, 98 Optical multiplexer, 100 Semiconductor manufacturing equipment.
Claims
1. A step of comparing a processing remaining amount of a film to be processed formed on a semiconductor wafer with a threshold value; a step of heating the semiconductor wafer while supplying an organic gas containing a substance having at least two substituents having an unshared electron pair in a molecule, thereby forming a compound between the film to be processed and the organic gas; a step of further heating the semiconductor wafer after the step of forming the compound to a predetermined temperature based on the result of the comparing step, thereby desorbing the compound from the surface of the semiconductor wafer; A method for manufacturing a semiconductor device comprising the steps of:
2. 2. The method for manufacturing a semiconductor device according to claim 1, wherein the step of desorbing the compound is a step of heating the semiconductor wafer in a plurality of stages to the predetermined temperature after stopping the supply of the organic gas when a processing remaining amount is equal to or less than a threshold value.
3. 2. The method for manufacturing a semiconductor device according to claim 1, wherein the step of desorbing the compound is a step of continuously increasing the temperature of the semiconductor wafer to the predetermined temperature while supplying the organic gas when a processing residual amount is larger than a threshold value.
4. The step of releasing the compound includes: a first desorption step of heating the semiconductor wafer in a plurality of stages to the predetermined temperature after stopping the supply of the organic gas when the amount of processing residue is equal to or less than a threshold value, thereby desorbing the compound; a second desorption step of heating the semiconductor wafer while supplying the organic gas and continuously raising the temperature to the predetermined temperature when the amount of processing residue is greater than a threshold value, thereby desorbing the compound; 2. The method for manufacturing a semiconductor device according to claim 1, wherein the compound forming step, the first desorption step, and the second desorption step are performed until the processing remaining amount is eliminated.
5. The organic gas has a phenol skeleton, and an OH group, an OCH 3 Group, OCOCH 3 Group, OCONH 2 group, NH2 group, N(CH 3 ) 2 2. The method for producing a semiconductor device according to claim 1, wherein the compound has one of the substituents selected from the group consisting of aryl, ... and aryl groups.
6. The organic gas has a phenol skeleton, and a CN group, CH═CH—CH, or the like is present at a position adjacent to a carbon atom to which an OH group is bonded. 3 group, CH=CH-CN group, CH=CH-CO 2 CH 3 2. The method for producing a semiconductor device according to claim 1, wherein the compound has one of the substituents selected from the group consisting of aryl, ... and aryl groups.
7. 7. The method for manufacturing a semiconductor device according to claim 6, wherein the organic gas contains 2-cyanophenol or o-hydroxycinnamic acid ester.
8. 2. The method for manufacturing a semiconductor device according to claim 1, wherein the organic gas is an aliphatic four-membered ring compound having a carbonyl group, and has an O atom as an electron-donating atom forming a four-membered ring with an O atom of the carbonyl group, and at least one carbon atom is arranged in the O atom.
9. The method for manufacturing a semiconductor device according to claim 8 , wherein the organic gas contains β-butyrolactone.
10. A semiconductor manufacturing apparatus comprising: a vacuum vessel having a processing chamber therein; a stage on which a semiconductor wafer having a film to be processed disposed inside the processing chamber is placed; a processing gas supply unit for supplying an organic gas into the processing chamber; an exhaust unit for exhausting the inside of the processing chamber; a heater for heating the semiconductor wafer to a predetermined temperature; and a control unit, The organic gas has at least two substituents having an unshared electron pair in the molecule, The control unit is a step of comparing a remaining amount of processing of the film to be processed with a threshold value; a step of forming a compound of the film to be processed and the organic gas by heating the semiconductor wafer while supplying the organic gas containing a substance having at least two substituents having an unshared electron pair in its molecule to the processing chamber; and a step of further heating the semiconductor wafer after the step of forming the compound based on a result of the comparing step, thereby raising the temperature to a predetermined temperature and desorbing the compound from the surface of the semiconductor wafer.
11. 11. The semiconductor manufacturing apparatus according to claim 10, wherein the step of desorbing the compound includes a step of heating the semiconductor wafer in a plurality of stages to the predetermined temperature after stopping the supply of the organic gas when a processing remaining amount is equal to or less than a threshold value.
12. 11. The semiconductor manufacturing apparatus according to claim 10, wherein the step of desorbing the compound includes the step of heating the semiconductor wafer while supplying the organic gas to the processing chamber to continuously raise the temperature to the predetermined temperature when a processing residual amount is greater than a threshold value.
Citation Information
Patent Citations
A novel method for atomic layer etching (ale) using sequential self-limiting thermal reactions.
JP2018500767A
Method for producing semiconductor
WO2021192210A1
Method for producing a semiconductor and device for producing a semiconductor
WO2022123725A1