Polymer composition, crosslinked product and tire
A polymer composition with specific structural units and a water-soluble component addresses the issue of low abrasion resistance and grip in winter tires, achieving improved wear resistance and ice grip performance.
Patent Information
- Application Number
- JP2020183168
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-30
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-10-30
AI Technical Summary
Conjugated diene polymers used in winter and all-season tires have low glass transition temperatures, resulting in soft vulcanized rubber with insufficient abrasion resistance and grip performance on ice.
A polymer composition comprising specific structural units and a conjugated diene polymer with a bond, combined with a water-soluble component, achieves a balance of good grip performance on ice and excellent wear resistance by controlling the composition ratio and incorporating additives.
The composition produces vulcanized rubber with enhanced abrasion resistance and grip on ice, while maintaining mechanical strength and reducing hardness changes due to heat aging.
Smart Images

Figure 0007569201000001 
Figure 0007569201000002 
Figure 0007569201000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polymer composition, a crosslinked product, and a tire. [Background technology]
[0002] Conjugated diene polymers such as styrene-butadiene copolymers have various good properties such as heat resistance, abrasion resistance, mechanical strength, moldability, etc., and are therefore widely used in various industrial products such as pneumatic tires, anti-vibration rubber, hoses, etc. In addition, various rubber materials have been proposed for use in winter tires to improve grip on road surfaces with large surface irregularities, such as icy road surfaces (for example, see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 2010-514867 Summary of the Invention [Problem to be solved by the invention]
[0004] In the manufacture of winter and all-season tires, polymers with relatively low glass transition temperatures (Tg) are generally used to obtain good grip performance on ice, and as a result, the resulting vulcanized rubber tends to be soft and not sufficiently wear-resistant.
[0005] The present invention has been made in consideration of the above problems, and has as its main object to provide a polymer composition from which vulcanized rubber having good grip performance on ice and excellent abrasion resistance can be produced. [Means for solving the problem]
[0006] The present inventors have conducted research to solve the above problems. As a result, they have found that the above problems can be solved by combining a specific conjugated diene polymer with a specific additive. According to the present invention, the following means are provided.
[0007] [1] A polymer composition comprising: (A) a conjugated diene-based polymer having a carbon-carbon unsaturated bond, in which the value θ represented by the following formula (i) is 0.75 or more, where p, q, r and s are the constituent ratios (molar ratios) in the polymer of a structural unit represented by the following formula (1), a structural unit represented by the following formula (2), a structural unit represented by the following formula (3), and a structural unit represented by the following formula (4), respectively; and (B) at least one component selected from the group consisting of water-soluble particles and water-soluble fibers. Formula (i): θ=(p+(0.5×r)) / (p+q+(0.5×r)+s) [ka] [2] A crosslinked product obtained by using the polymer composition of [1] above. [3] A tire having a tread and / or a sidewall formed from the polymer composition of [1] above. Effect of the Invention
[0008] According to the present invention, it is possible to produce a vulcanized rubber which exhibits good grip performance on ice and is excellent in abrasion resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] <Polymer composition> The polymer composition of the present invention (hereinafter, also simply referred to as "the composition") contains the following components (A) and (B). Each component contained in the composition, and components that are blended as necessary, are described below. In this specification, a numerical range described using "to" means that the numerical values before and after "to" are included as the lower and upper limits.
[0010] <(A) Conjugated diene polymer> The component (A) is a conjugated diene-based polymer having a carbon-carbon unsaturated bond (hereinafter also referred to as “polymer (A)”), in which the value θ represented by the following formula (i) is 0.75 or more, where p, q, r, and s are the constituent ratios (molar ratios) in the polymer of a structural unit represented by the following formula (1), a structural unit represented by the following formula (2), a structural unit represented by the following formula (3), and a structural unit represented by the following formula (4), respectively. Formula (i): θ=(p+(0.5×r)) / (p+q+(0.5×r)+s)
[0011] As the polymer (A), a hydrogenated product of a polymer having a structural unit derived from a conjugated diene compound can be used. Such a polymer (A) can be produced by first polymerizing a monomer containing a conjugated diene compound to obtain an unhydrogenated conjugated diene-based polymer, and then hydrogenating the obtained polymer.
[0012] As the conjugated diene compound constituting the (A) polymer, 1,3-butadiene can be preferably used. In addition, in the polymerization for obtaining the (A) polymer, in addition to 1,3-butadiene, a conjugated diene compound other than 1,3-butadiene may be used. Specific examples of the conjugated diene compound other than 1,3-butadiene include isoprene, 2,3-dimethyl-1,3-butadiene, and 1,3-pentadiene. Among these, isoprene is preferable as the conjugated diene compound other than 1,3-butadiene. In addition, when producing the (A) polymer, one type of compound may be used alone as the conjugated diene compound, or two or more types of compounds may be used in combination.
[0013] From the viewpoint of increasing the strength of the crosslinked body obtained by using the present composition, the (A) polymer is preferably a copolymer of a conjugated diene compound and an aromatic vinyl compound. Examples of aromatic vinyl compounds used in polymerization include styrene, 2-methylstyrene, 3-methylstyrene, 4-methylstyrene, α-methylstyrene, N,N-dimethylaminoethylstyrene, and diphenylethylene. Among these, at least one of styrene and α-methylstyrene is particularly preferably used as the aromatic vinyl compound. The aromatic vinyl compounds can be used alone or in combination of two or more.
[0014] When the polymer (A) is a copolymer of a conjugated diene compound and an aromatic vinyl compound, it is preferably a copolymer of 1,3-butadiene and styrene, because it has high living properties in anionic polymerization. The polymer (A) is preferably a random copolymer in which the distribution of the conjugated diene compound and the aromatic vinyl compound is irregular, because it can improve the dispersibility of the filler blended in the polymer composition. The random copolymer of the conjugated diene compound and the aromatic vinyl compound may further have a block portion made of a conjugated diene compound or an aromatic vinyl compound, as long as the effects of the present invention are obtained.
[0015] In the copolymer of a conjugated diene compound and an aromatic vinyl compound, the content of structural units derived from the aromatic vinyl compound is preferably 3 to 45% by mass based on the total amount of monomers constituting the copolymer, from the viewpoint of improving strength, abrasion resistance, and low hysteresis loss properties, as well as improving grip performance on ice. The content of structural units derived from the aromatic vinyl compound is more preferably 4% by mass or more, and even more preferably 5% by mass or more, based on the total amount of monomers constituting the copolymer.
[0016] In addition, the content of the structural unit derived from the aromatic vinyl compound is more preferably 40% by mass or less, even more preferably 35% by mass or less, even more preferably 30% by mass or less, and particularly preferably 25% by mass or less, based on the total amount of monomers constituting the copolymer, in order to sufficiently increase the grip performance on ice. By setting the content of the aromatic vinyl compound unit within the above range, it is possible to achieve both productivity, strength, and abrasion resistance. It is preferable that the (A) polymer contains 50 to 97% by mass of 1,3-butadiene units, 3 to 45% by mass of aromatic vinyl compound units, and 0 to 30% by mass of conjugated diene compound units other than 1,3-butadiene, based on 100% by mass of the total amount of monomers constituting the (A) polymer. By setting such a blending ratio, it is preferable to maintain high abrasion resistance of the crosslinked body while improving the grip performance on ice in a well-balanced manner.
[0017] The conjugated diene compounds and aromatic vinyl compounds exemplified above all have the same effect in that they can produce a conjugated diene polymer having an active terminal. Therefore, even if a compound is not described in the examples described later, it can be used in the present invention.
[0018] In the polymerization, other monomers than the conjugated diene compound and the aromatic vinyl compound can be used. Examples of the other monomers include acrylonitrile, methyl (meth)acrylate, and ethyl (meth)acrylate. The content of the structural unit derived from the other monomer is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 10% by mass or less, based on the total amount of the monomers constituting the (A) polymer.
[0019] As the polymerization method for obtaining the (A) polymer, any of solution polymerization, gas phase polymerization, and bulk polymerization may be used, but solution polymerization is particularly preferred. As the polymerization form, any of batch and continuous methods may be used. When using the solution polymerization method, a specific example of the polymerization method is a method in which a monomer containing a conjugated diene compound is polymerized in an organic solvent in the presence of a polymerization initiator and a randomizer that is used as necessary.
[0020] As the polymerization initiator, at least one of an alkali metal compound and an alkaline earth metal compound can be used. As the alkali metal compound and the alkaline earth metal compound, those usually used as initiators for anionic polymerization can be used. Specific examples of the polymerization initiator include methyl lithium, ethyl lithium, n-propyl lithium, n-butyl lithium, sec-butyl lithium, t-butyl lithium, 1,4-dilithiobutane, phenyl lithium, stilbene lithium, naphthyl lithium, naphthyl sodium, naphthyl potassium, di-n-butyl magnesium, di-n-hexyl magnesium, ethoxy potassium, calcium stearate, and the like. Among these, lithium compounds can be preferably used as the polymerization initiator.
[0021] The polymerization reaction may be carried out in the presence of a compound (hereinafter also referred to as "initiation modifier") obtained by mixing at least one of the above-mentioned alkali metal compounds and alkaline earth metal compounds with a compound having a functional group that interacts with silica. By carrying out polymerization in the presence of the initiation modifier, a functional group that interacts with silica can be introduced to the polymerization initiation terminal of the (A) polymer. In addition, by introducing a functional group that interacts with silica to the initiation terminal of the (A) polymer, it is preferable in that the low hysteresis loss performance (low fuel consumption performance) of the vulcanized rubber obtained using this composition can be improved.
[0022] In this specification, "interaction" means forming a covalent bond between molecules or forming an intermolecular force weaker than a covalent bond (for example, an electromagnetic force acting between molecules such as an ion-dipole interaction, a dipole-dipole interaction, a hydrogen bond, or a van der Waals force). The "functional group that interacts with silica" is a group having at least one atom that interacts with silica (for example, a nitrogen atom, a sulfur atom, a phosphorus atom, an oxygen atom, a silicon atom, etc.). The silicon atom of the "functional group that interacts with silica" is preferably a silicon atom in a hydrocarbyloxysilyl group.
[0023] The initiator modifier is preferably a reaction product of a lithium compound such as an alkyl lithium and a nitrogen-containing compound such as a secondary amine compound. Examples of the nitrogen-containing compound include dimethylamine, diethylamine, dipropylamine, dibutylamine, dodecamethyleneimine, N,N'-dimethyl-N'-trimethylsilyl-1,6-diaminohexane, piperidine, pyrrolidine, hexamethyleneimine, heptamethyleneimine, dicyclohexylamine, N-methylbenzylamine, di-(2-ethylhexyl)amine, diallylamine, morpholine, N-(trimethylsilyl)piperazine, N-(tert-butyldimethylsilyl)piperazine, and 1,3-ditrimethylsilyl-1,3,5-triazinane.
[0024] When polymerization is carried out in the presence of an initiating modifier, an alkali metal compound or an alkaline earth metal compound may be mixed with a nitrogen-containing compound in advance to prepare an initiating modifier, and the prepared modifier may be added to the polymerization system to carry out polymerization. Alternatively, an alkali metal compound or an alkaline earth metal compound and a nitrogen-containing compound may be added to the polymerization system, and the two may be mixed in the polymerization system to prepare an initiating modifier, and then polymerization may be carried out.
[0025] The randomizer can be used for the purpose of adjusting the content of 1,2-vinyl bonds (vinyl content) in the polymer obtained by the above polymerization. Examples of the randomizer include dimethoxybenzene, tetrahydrofuran, dimethoxyethane, diethylene glycol dibutyl ether, diethylene glycol dimethyl ether, 2,2-di(tetrahydrofuryl)propane, 2-(2-ethoxyethoxy)-2-methylpropane, triethylamine, pyridine, N-methylmorpholine, and tetramethylethylenediamine. The randomizer can be used alone or in combination of two or more.
[0026] The organic solvent used in the polymerization may be any organic solvent inert to the reaction, and may be, for example, an aliphatic hydrocarbon, an alicyclic hydrocarbon, an aromatic hydrocarbon, etc. Among them, a hydrocarbon having 3 to 8 carbon atoms is preferable, and specific examples thereof include, for example, n-pentane, isopentane, n-hexane, cyclohexane, propene, 1-butene, isobutene, trans-2-butene, cis-2-butene, 1-hexene, 2-hexene, benzene, toluene, xylene, ethylbenzene, heptane, cyclopentane, methylcyclopentane, methylcyclohexane, 1-pentene, 2-pentene, cyclohexene, etc. The organic solvent may be used alone or in combination of two or more.
[0027] When solution polymerization is used, the monomer concentration in the reaction solvent is preferably 5 to 50% by mass, more preferably 10 to 30% by mass, from the viewpoint of maintaining a balance between productivity and ease of polymerization control. The temperature of the polymerization reaction is preferably -20 to 150°C, more preferably 0 to 120°C, and particularly preferably 20 to 100°C. The polymerization reaction is preferably carried out under a pressure sufficient to keep the monomer substantially in a liquid phase. Such a pressure can be obtained by a method such as pressurizing the inside of a reactor with a gas inert to the polymerization reaction.
[0028] The 1,2-vinyl content (vinyl content) of the conjugated diene polymer obtained by the above polymerization is preferably 5 to 70 mol %. When the vinyl content is 5 mol % or more, the grip property tends to be good, and when it is 70 mol % or less, the abrasion resistance tends to be good. From this viewpoint, the vinyl content is more preferably 10 mol % or more, and even more preferably 15 mol % or more. Moreover, the vinyl content is more preferably 60 mol % or less, and even more preferably 50 mol % or less. The vinyl content is 1 The values were measured by H-NMR.
[0029] The above polymerization can provide a conjugated diene polymer having an active terminal. When terminating the polymerization, the conjugated diene polymer having an active terminal may be reacted with a polymerization terminator such as alcohol or hydrogen or a coupling agent. Alternatively, the conjugated diene polymer having an active terminal may be reacted with a compound having a functional group that interacts with silica (hereinafter also referred to as a "terminal modifier"). By reacting the conjugated diene polymer having an active terminal with a terminal modifier, a modified conjugated diene polymer having a polymerization end modified with a functional group that interacts with silica can be obtained as the (A) polymer. In addition, by using a polymer having a functional group that interacts with silica introduced into the polymerization end as the (A) polymer, it is preferable in that low hysteresis loss performance can be improved. In particular, the (A) polymer preferably has at least one functional group selected from the group consisting of an amino group, a nitrogen-containing heterocyclic group, a phosphino group, a hydroxyl group, a thiol group, and a hydrocarbyloxysilyl group. In this specification, the term "active end" refers to a portion (more specifically, a metal end) that is present at the end of a molecular chain and is other than a structure derived from a monomer having a carbon-carbon double bond.
[0030] The terminal modifier is not particularly limited as long as it has a functional group that interacts with silica and can react with the active terminal of the conjugated diene polymer. Among them, the terminal modifier is preferably a compound having one atom selected from the group consisting of nitrogen atom, sulfur atom, phosphorus atom, oxygen atom and silicon atom, and having no active hydrogen bonded to the atom. In particular, the terminal modifier is preferably a compound having one or more functional groups selected from the group consisting of amino group, group having carbon-nitrogen double bond, nitrogen-containing heterocyclic group, phosphino group, cyclic ether group, cyclic thioether group, protected hydroxyl group, protected thiol group and hydrocarbyloxysilyl group, and capable of reacting with the polymerization active terminal. The amino group is preferably a protected primary amino group, secondary amino group, or tertiary amino group.
[0031] As the terminal modifying agent, at least one selected from the group consisting of compounds represented by the following formula (5) and compounds represented by the following formula (6) can be preferably used. [ka] (In formula (5), A 1 has at least one atom selected from the group consisting of nitrogen, phosphorus, oxygen, sulfur, and silicon, has no active hydrogen, and R 5 R is a monovalent functional group bonded to a nitrogen atom, a phosphorus atom, an oxygen atom, a sulfur atom, a silicon atom, or a carbon atom contained in a carbonyl group, or is a (thio)epoxy group. 3 and R 4 are each independently a hydrocarbyl group. 5 is a hydrocarbylene group. r is an integer of 0 to 2. However, when r is 2, multiple R 3 are the same or different groups. When r is 0 or 1, multiple R 4 are the same or different groups. [ka] (In formula (6), A 2has at least one atom selected from the group consisting of nitrogen, phosphorus, oxygen, sulfur, and silicon, has no active hydrogen, and R 9 R is a monovalent functional group bonded to R via a nitrogen atom, phosphorus atom, oxygen atom, sulfur atom or silicon atom, or a hydrocarbyl group having 1 to 20 carbon atoms. 6 and R 7 are each independently a hydrocarbyl group. 8 is a hydrocarbylene group. 9 is a single bond or a hydrocarbylene group. m is 0 or 1. However, when m is 0, multiple R 7 are the same or different groups.
[0032] In the above formula (5) and formula (6), R 3 , R 4 , R 6 , R 7 and A when it is a hydrocarbyl group. 2 Regarding the above, the hydrocarbyl group is preferably a linear or branched alkyl group having 1 to 20 carbon atoms, a cycloalkyl group having 3 to 20 carbon atoms, or an aryl group having 6 to 20 carbon atoms. R 5 and R 9 The hydrocarbylene group in R is preferably a linear or branched alkanediyl group having 1 to 20 carbon atoms, a cycloalkylene group having 3 to 20 carbon atoms, or an arylene group having 6 to 20 carbon atoms. 8 The hydrocarbylene group is preferably a linear or branched alkanediyl group having 1 to 20 carbon atoms. r is preferably 0 or 1 from the viewpoint of increasing the reactivity with the conjugated diene polymer. A 1 When A is the monovalent functional group, 1 At least one atom selected from the group consisting of nitrogen, phosphorus, oxygen, sulfur and silicon, and 2 When A is a monovalent functional group, 2At least one atom selected from the group consisting of nitrogen, phosphorus, oxygen, sulfur and silicon contained in A may be protected with a protecting group (e.g., a tri-substituted hydrocarbylsilyl group, etc.). In this specification, active hydrogen refers to a hydrogen atom bonded to an atom other than a carbon atom, and preferably refers to a hydrogen atom having a bond energy lower than that of the carbon-hydrogen bond of polymethylene. The protecting group is a 1 , A 2 is a functional group that converts the functional group into an inactive functional group toward the polymerization active terminal. The (thio)epoxy group includes an epoxy group and a thioepoxy group.
[0033] A 1 may be a group that can be converted to an onium ion by an onium salt generating agent. 1 ) can impart excellent shape retention to the polymer (A). 1 Specific examples of the include a nitrogen-containing group in which two hydrogen atoms of a primary amino group are replaced by two protective groups, a nitrogen-containing group in which one hydrogen atom of a secondary amino group is replaced by one protective group, a tertiary amino group, an imino group, a pyridyl group, a phosphorus-containing group in which two hydrogen atoms of a primary phosphino group are replaced by two protective groups, a phosphorus-containing group in which one hydrogen atom of a secondary phosphino group is replaced by one protective group, a tertiary phosphino group, an epoxy group, a thioepoxy group, a group in which the hydrogen atom of a hydroxyl group is replaced by a protective group, a sulfur-containing group in which the hydrogen atom of a thiol group is replaced by a protective group, a hydrocarbyloxycarbonyl group, etc. Among these, a group having a nitrogen atom is preferable in terms of good affinity with silica, and a tertiary amino group or a nitrogen-containing group in which two hydrogen atoms of a primary amino group are replaced by two protective groups is more preferable.
[0034] Preferable specific examples of the terminal modifying agent include compounds represented by the above formula (5), such as N,N-bis(trimethylsilyl)aminopropyltrimethoxysilane, N,N-bis(trimethylsilyl)aminopropylmethyldiethoxysilane, N,N',N'-tris(trimethylsilyl)-N-(2-aminoethyl)-3-aminopropyltriethoxysilane, 3-(4-trimethylsilyl-1-piperazino)propylmethyldimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 3-glycidoxypropyltriethoxysilane.
[0035] Specific examples of the compound represented by the above formula (6) include, for example, 2,2-dimethoxy-1-(3-trimethoxysilylpropyl)-1,2-azasilolidine, 2,2-diethoxy-1-(3-trimethoxysilylpropyl)-1,2-azasilolidine, 2,2-dimethoxy-1-phenyl-1,2-azasilolidine, 1-trimethylsilyl-2,2-dimethoxy-1-aza-2-silacyclopentane, 2-(2,2-dimethoxy-1,2-azasilolidine-1-yl)-N,N-diethylethane-1-amine, 2-(2,2-dimethoxy-1,2-azasilolidine-1-yl)-N,N-dimethylethane-1-amine, and 3-(2,2-dimethoxy-1,2-azasilolidine-1-yl)-N,N-diethylpropan-1-amine. The terminal modifying agent may be used alone or in combination of two or more kinds.
[0036] The above-mentioned terminal modification reaction can be carried out, for example, as a solution reaction. This solution reaction may be carried out using a solution containing unreacted monomers after the completion of the polymerization reaction, or may be carried out after isolating the conjugated diene polymer contained in the solution and dissolving it in a suitable solvent such as cyclohexane. The terminal modification reaction may be carried out using either a batch system or a continuous system. In this case, the method of adding the terminal modifier is not particularly limited, and examples thereof include a method of adding the terminal modifier all at once, a method of adding the terminal modifier in portions, and a method of adding the terminal modifier continuously.
[0037] The amount of the terminal modification agent used may be appropriately set according to the type of compound used in the reaction, but is preferably 0.1 molar equivalent or more, more preferably 0.3 molar equivalent or more, relative to the metal atom of the polymerization initiator involved in the polymerization reaction. By setting the amount of the terminal modification agent to 0.1 molar equivalent or more, the modification reaction can be sufficiently advanced, which is preferable in that the effect of improving the dispersibility of silica can be enhanced. The temperature of the terminal modification reaction is usually the same as the temperature of the polymerization reaction, and is preferably -20 to 150 ° C, more preferably 0 to 120 ° C, and particularly preferably 20 to 100 ° C. If the temperature of the modification reaction is too low, the viscosity of the modified conjugated diene polymer tends to increase. In addition, if the temperature of the modification reaction is too high, the polymerization active terminal is easily deactivated. The time of the terminal modification reaction is preferably 1 minute to 5 hours, more preferably 2 minutes to 1 hour.
[0038] For the purpose of adjusting the Mooney viscosity of the polymer (A), a coupling agent such as silicon tetrachloride or a polyfunctional epoxy compound (e.g., tetraglycidyl-1,3-bisaminomethylcyclohexane, etc.) may be reacted with the conjugated diene polymer having an active terminal before or after the modification reaction using the terminal modifier, or simultaneously with the modification reaction using the terminal modifier. The amount of the coupling agent used can be appropriately set depending on the desired Mooney viscosity of the polymer (A) and the compounds used in the reaction, but it is preferably 0.01 to 0.8 molar equivalents relative to the metal atoms of the polymerization initiator involved in the polymerization reaction. The coupling agent may be used alone or in combination of two or more.
[0039] Subsequently, the modified or unmodified conjugated diene polymer obtained above can be hydrogenated to obtain the polymer (A). The hydrogenation reaction method and conditions may be any method and conditions that can obtain a conjugated diene polymer with a desired hydrogenation rate (hydrogenation rate). Examples of hydrogenation methods include a method using a catalyst mainly composed of an organometallic compound of titanium as a hydrogenation catalyst, a method using a catalyst composed of an organic compound of iron, nickel, or cobalt and an organometallic compound such as alkylaluminum, a method using an organic complex of an organometallic compound such as ruthenium or rhodium, and a method using a catalyst in which a metal such as palladium, platinum, ruthenium, cobalt, or nickel is supported on a carrier such as carbon, silica, or alumina. Among the various methods, a method in which hydrogenation is performed under mild conditions of low pressure and low temperature using a homogeneous catalyst composed of an organometallic compound of titanium alone or an organometallic compound of titanium and an organometallic compound of lithium, magnesium, or aluminum (JP-B-63-4841, JP-B-1-37970) is industrially preferred. In addition, the hydrogenation selectivity to the double bonds of butadiene is high, which is suitable for the purpose of the present invention.
[0040] The hydrogenation of the conjugated diene polymer is carried out in a solvent which is inactive to the catalyst and which the conjugated diene polymer is soluble in. Preferred solvents include aliphatic hydrocarbons such as n-pentane, n-hexane, and n-octane, alicyclic hydrocarbons such as cyclohexane and cycloheptane, aromatic hydrocarbons such as benzene and toluene, and ethers such as diethyl ether and tetrahydrofuran, either alone or as a mixture mainly composed of these.
[0041] The hydrogenation reaction is generally carried out by maintaining the conjugated diene polymer at a predetermined temperature under hydrogen or an inert atmosphere, adding a hydrogenation catalyst with or without stirring, and then introducing hydrogen gas to pressurize to a predetermined pressure. The inert atmosphere means an atmosphere that does not react with the participants in the hydrogenation reaction, and examples of such an atmosphere include helium, neon, and argon. Air and oxygen are not preferred because they oxidize the catalyst and cause deactivation of the catalyst. Nitrogen is also not preferred because it acts as a catalyst poison during the hydrogenation reaction and reduces the hydrogenation activity. In particular, it is most suitable that the hydrogenation reactor has an atmosphere of hydrogen gas alone.
[0042] The hydrogenation reaction process for obtaining the hydrogenated conjugated diene polymer may be a batch process, a continuous process, or a combination thereof. When a titanocene diaryl compound is used as the hydrogenation catalyst, it may be added to the reaction solution as it is, or may be added as a solution in an inert organic solvent. When the catalyst is used as a solution, various solvents that do not react with the participants in the hydrogenation reaction may be used as the inert organic solvent. The inert organic solvent is preferably the same solvent as that used in the hydrogenation reaction. The amount of the catalyst added is 0.02 to 20 mmol per 100 g of the conjugated diene polymer before hydrogenation.
[0043] The (A) polymer has a value θ represented by the following formula (i) of 0.75 or more. By making θ 0.75 or more, it is possible to obtain a crosslinked body having sufficiently high abrasion resistance and suppressing hardness change due to thermal aging. For these reasons, θ is preferably 0.78 or more, more preferably 0.80 or more, and even more preferably 0.85 or more. Moreover, from the viewpoint of allowing the crosslinking reaction to proceed sufficiently, θ is preferably 0.99 or less, and more preferably 0.97 or less. Formula (i): θ=(p+(0.5×r)) / (p+q+(0.5×r)+s)
[0044] The above formula (i) represents the hydrogenation rate of the conjugated diene polymer. That is, the value θ defined by the above formula (i) corresponds to the hydrogenation rate of the (A) polymer. Therefore, for example, when θ is 0.75, this is equivalent to the hydrogenation rate of the (A) polymer being 75%. The hydrogenation rate in the polymer can be adjusted by the hydrogenation reaction time, etc. The hydrogenation rate is 1 The values were measured by H-NMR.
[0045] A preferred method for obtaining polymer (A) is to solution polymerize a monomer containing 1,3-butadiene in the presence of an alkali metal compound, and then use the resulting polymer solution as is to carry out a terminal modification reaction, followed by subjecting the resulting polymer solution to a hydrogenation reaction, which is industrially useful. In this case, polymer (A) can be obtained by removing the solvent from the solution obtained above and isolating the polymer. The isolation of the polymer can be carried out by a known method for removing the solvent, such as steam stripping, and a drying operation, such as heat treatment.
[0046] The weight average molecular weight (Mw) of the polymer (A) is preferably 1.0×10 5 ~2.0×10 6 Mw is 1.0×10 5 When the Mw is 2.0×10 or more, the abrasion resistance and fuel economy of the obtained crosslinked body can be sufficiently improved. 6 The Mw of the polymer (A) is preferably 1.0×10 or less, which is preferable in terms of improving the processability of the present composition. 5 More preferably, it is 1.2×10 5 The Mw of the polymer (A) is more preferably 1.5×10 6 More preferably, it is 1.5×10 6 The weight average molecular weight in this specification is a polystyrene-equivalent value measured by gel permeation chromatography (GPC), and represents the weight average molecular weight based on all peaks (total weight average molecular weight).
[0047] From the viewpoint of obtaining a crosslinked product having excellent grip performance on ice, the glass transition temperature (Tg) of the polymer (A) is preferably −20° C. or lower, more preferably −30° C. or lower, even more preferably −40° C. or lower, and even more preferably −45° C. or lower. The Tg of the polymer (A) is, for example, −70° C. or higher. In this specification, the Tg of the polymer is a value measured by differential scanning calorimetry (DSC) in accordance with ASTM D3418.
[0048] From the viewpoint of obtaining a crosslinked product with excellent grip performance on ice, it is preferable that the Tg of the polymer (A) is low, but compared with non-hydrogenated SBR having a similar Tg, the polymer (A) has good abrasion resistance but room for improvement in grip performance on ice. In this regard, a polymer composition containing the polymer (A) and the component (B) (water-soluble component) is preferable because it is possible to obtain a vulcanized rubber with a good balance between abrasion resistance and grip performance on ice, even when the polymer (A) having a relatively low Tg is used.
[0049] <(B) Water-soluble component> The component (B) blended in the present composition is at least one selected from the group consisting of water-soluble particles and water-soluble fibers (hereinafter also referred to as "water-soluble component (B)"). The water-soluble component (B) is not particularly limited as long as it is soluble or swellable in water at room temperature, but for example, a substance having a solubility of 1.2 g / 100 g-H2O or more in water at 25°C can be used.
[0050] ·Water-soluble particles The water-soluble particles include water-soluble inorganic particles and organic particles. Among these, the water-soluble inorganic particles include, for example, particles of chlorides such as sodium chloride, potassium chloride, magnesium chloride, etc., sulfides such as sodium sulfate, potassium sulfate, magnesium sulfate, etc., carbonates such as sodium carbonate, sodium hydrogen carbonate, etc., phosphates such as sodium hydrogen phosphate, etc., hydroxides such as sodium hydroxide, potassium hydroxide, etc.
[0051] Examples of water-soluble organic particles include particles of lignin sulfonates such as sodium lignin sulfonate, potassium lignin sulfonate, calcium lignin sulfonate, magnesium lignin sulfonate, and ammonium lignin sulfonate; resins such as polyvinyl alcohol or derivatives thereof (e.g., partial acetates, carboxylic acid-modified polyvinyl alcohol, and sulfonic acid-modified polyvinyl alcohol), alkali salts of poly(meth)acrylic acid, and alkali salts of (meth)acrylic acid / (meth)acrylic acid ester copolymers; and sugars such as monosaccharides, oligosaccharides, and polysaccharides.
[0052] Specific examples of sugars include monosaccharides such as glucose, fructose, galactose, etc., oligosaccharides such as sucrose, lactose, maltose, raffinose, maltotriose, trehalose, palatinose, etc., and polysaccharides such as starch, dextrin, glycogen, glucan, xanthan gum, galactomannan (guar gum, fenugreek gum, etc.), cyclodextrin (α-cyclodextrin, β-cyclodextrin, γ-cyclodextrin, etc.), methylcellulose, ethylcellulose, carboxymethylcellulose, etc. As the water-soluble particles, one of these can be used alone or two or more can be used in combination.
[0053] The water-soluble particles may be in various forms, such as powder, granules, microbeads, etc. The water-soluble particles used as the (B) water-soluble component are preferably solid water-soluble particles. From the viewpoint of obtaining a sufficient effect of improving grip performance on ice, the water-soluble particles preferably have a median particle size of 1 μm or more, more preferably 2 μm or more. From the viewpoint of achieving a good balance between grip performance on ice and abrasion resistance, the median particle size is preferably 1000 μm or less, more preferably 500 μm or less. In this specification, the median particle size of the water-soluble particles is the median diameter (D50), which is a value measured by a laser diffraction / scattering method.
[0054] Soluble fiber As the water-soluble fiber, short fibers that can be dissolved or swelled in water can be used. Specifically, the fiber length of the water-soluble fiber is preferably 1 mm or more, more preferably 2 mm or more, and even more preferably 4 mm or more, from the viewpoint of obtaining a sufficient effect of improving grip performance on ice. In addition, the fiber length is preferably 30 mm or less, more preferably 20 mm or less, and even more preferably 15 mm or less, from the viewpoint of suppressing a decrease in abrasion resistance and processability. The diameter (average diameter) of the water-soluble fiber is preferably 5 μm or more, more preferably 10 μm or more. In addition, the average diameter of the water-soluble fiber is preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 20 μm or less.
[0055] Examples of the water-soluble fiber include fibers that mainly contain the substances exemplified in the description of the water-soluble organic particles. As the water-soluble fiber, at least one selected from the group consisting of polyvinyl alcohol fibers and polysaccharide fibers can be preferably used. As the water-soluble fiber, one of these may be used alone, or two or more may be used in combination.
[0056] The content of the water-soluble component (B) in the composition is not particularly limited as long as the effect of the present invention can be obtained, but is preferably 0.1 parts by mass or more and 40 parts by mass or less relative to 100 parts by mass of the polymer (A). If the content of the water-soluble component (B) is in the above range, it is preferable that a vulcanized rubber that exhibits good ice grip performance while ensuring abrasion resistance can be obtained. From this viewpoint, the content of the water-soluble component (B) is more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more, relative to 100 parts by mass of the polymer (A). In addition, from the viewpoint of suppressing the decrease in abrasion resistance of the crosslinked body, the content of the water-soluble component (B) is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, even more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the polymer (A).
[0057] Here, when a water-soluble component (B) is blended into a polymer composition (hereinafter also referred to as a "rubber composition") for obtaining a vulcanized rubber to produce a pneumatic tire, the water-soluble component (B) dissolves in water to form surface irregularities on the contact surface of the vulcanized rubber with water, which can improve grip performance on ice. However, when the water-soluble component (B) is blended into the rubber composition, there is a concern that the abrasion resistance of the resulting vulcanized rubber will be significantly reduced. In addition, rubber compositions generally tend to harden due to deterioration over time, resulting in a decrease in grip performance. In contrast, the present composition, which is blended with the polymer (A) and the water-soluble component (B), can produce a vulcanized rubber with a good balance between abrasion resistance and grip performance on ice. The present composition is also suitable for producing winter tires or all-season tires.
[0058] <Other ingredients> In addition to the (A) polymer and the (B) water-soluble component, the present composition may further contain the following components.
[0059] ·Porous particles The composition may further contain porous particles (hereinafter also referred to as "(C) porous particles"). When the composition further contains porous particles, it is possible to improve the friction force on ice. Therefore, the composition in which the (C) porous particles are blended together with the (B) water-soluble component is particularly suitable for manufacturing winter tires or all-season tires. The (B) water-soluble component differs from the (C) porous particles in that it does not have a porous structure.
[0060] (C) Porous particles include water-soluble or water-insoluble inorganic particles and organic particles. The inorganic particles are not particularly limited as long as they are porous, but among them, metal oxide particles can be preferably used, and porous metal oxide particles having at least one metal atom selected from the group consisting of aluminum, silicon, and titanium can be more preferably used. Specific examples of metal oxides constituting such porous particles include aluminum oxide (alumina), aluminum hydroxide, silicon dioxide, silicon hydroxide, aluminosilicates (e.g., sodium aluminosilicate, potassium aluminosilicate, calcium aluminosilicate, etc.), titanium oxide, etc. Among these, porous particles composed of at least one metal atom selected from the group consisting of aluminosilicates and glass can be preferably used.
[0061] As the organic particles, at least one selected from the group consisting of porous resin particles and porous polysaccharide particles can be preferably used. Examples of materials constituting the porous resin particles include polyamide (nylon 6, nylon 6,6, nylon 11, nylon 12, nylon 66, etc.), polyether, polyester, olefin polymers (polyethylene, polypropylene, polystyrene, ethylene-vinyl acetate copolymer, etc.), (meth)acrylic polymers, vinyl polymers (polyvinyl chloride, polyvinyl acetate, etc.), etc. Examples of polysaccharides constituting the porous polysaccharide particles include the polysaccharides exemplified in the explanation of the water-soluble organic particles, and water-insoluble polysaccharides such as cellulose and chitin. As the porous organic particles, among others, porous polyamide particles, porous (meth)acrylic polymers, porous cellulose particles, porous chitin particles, etc. can be preferably used.
[0062] The particle size of the (C) porous particles is not particularly limited, but from the viewpoint of obtaining a sufficient effect of improving grip performance on ice, the median particle size is preferably 1 μm or more, more preferably 5 μm or more. Also, from the viewpoint of suppressing a decrease in the strength and abrasion resistance of the obtained vulcanized rubber, the median particle size of the (C) porous particles is preferably 2000 μm or less, more preferably 1000 μm or less. In this specification, the median particle size of the (C) porous particles is the median diameter (D50), which is a value measured by a laser diffraction / scattering method.
[0063] In the present composition, the content of the (C) porous particles is not particularly limited as long as the effects of the present invention can be obtained, but is preferably 0.5 parts by mass or more and 40 parts by mass or less relative to 100 parts by mass of the (A) polymer. By setting the content of the (C) porous particles in the above range, it is preferable that the grip performance on ice can be sufficiently improved while maintaining good strength and abrasion resistance. From this viewpoint, the content of the (C) porous particles is more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more, relative to 100 parts by mass of the (A) polymer. In addition, from the viewpoint of suppressing the decrease in the strength and abrasion resistance of the crosslinked body, the content of the (C) porous particles is preferably 30 parts by mass or less, and more preferably 25 parts by mass or less, relative to 100 parts by mass of the (A) polymer.
[0064] Other rubber components The present composition may contain only the (A) polymer as a rubber component, but may also contain a rubber component different from the (A) polymer (hereinafter also referred to as "other rubber component") in addition to the (A) polymer, within a range that does not impair the effects of the present invention. The type of such other rubber component is not particularly limited, and examples thereof include styrene butadiene rubber (SBR), butadiene rubber (BR. For example, high cis BR having 90% or more cis-1,4 bonds, BR containing syndiotactic-1,2-polybutadiene (SPB), etc.), isoprene rubber (IR), styrene isoprene copolymer rubber, butadiene isoprene copolymer rubber, natural rubber (NR), halogenated rubber, etc. The other rubber component is more preferably SBR, BR, and NR. The amount of the other rubber component is preferably 60% by mass or less, more preferably 40% by mass or less, based on the total amount of the rubber components ((A) polymer and other rubber components) contained in the polymer composition.
[0065] In this specification, the "rubber component" contained in the polymer composition refers to a polymer that can be thermally cured to obtain a cured product exhibiting rubber elasticity. The cured product exhibits the property of undergoing large deformation under small force at room temperature (for example, deformation that is more than twice the size when stretched at room temperature) and rapidly returning to almost the original shape when the force is removed.
[0066] Silica, etc. The present composition preferably contains at least one selected from the group consisting of silica and carbon black (hereinafter also referred to as "silica, etc."). Silica is preferred in that it provides a good static-dynamic ratio and low hysteresis loss properties, and carbon black is preferred in that it has a high effect of improving the strength of the polymer composition and vulcanized rubber. Examples of silica include wet silica (hydrated silicic acid), dry silica (anhydrous silicic acid), colloidal silica, etc., of which wet silica is preferred. Examples of carbon black include furnace black, acetylene black, thermal black, channel black, graphite, etc., of which furnace black is preferred.
[0067] In the present composition, the total amount of silica and carbon black is preferably 40 to 150 parts by mass relative to 100 parts by mass of the rubber component contained in the polymer composition. When the amount of silica, etc. is 40 parts by mass or more, it is preferable in that the effect of improving the strength of the vulcanized rubber can be sufficiently obtained. In addition, when the amount of silica, etc. is 150 parts by mass or less, it is preferable in that the abrasion resistance of the vulcanized rubber can be sufficiently ensured. The amount of silica, etc. is preferably 50 parts by mass or more, more preferably 55 parts by mass or more, relative to 100 parts by mass of the total amount of the rubber component. In addition, the amount of silica, etc. is preferably 150 parts by mass or less, more preferably 140 parts by mass or less, relative to 100 parts by mass of the total amount of the rubber component.
[0068] Crosslinking agent The composition preferably contains a crosslinking agent. The type of crosslinking agent used is not particularly limited. Specific examples of the crosslinking agent include organic peroxides, phenolic resins, sulfur, sulfur compounds, p-quinone, p-quinone dioxime derivatives, bismaleimide compounds, epoxy compounds, silane compounds, amino resins, polyols, polyamines, triazine compounds, metal soaps, etc. Among these, the crosslinking agent used is preferably at least one selected from the group consisting of organic peroxides, phenolic resins, and sulfur. The crosslinking agent may be used alone or in combination of two or more.
[0069] Examples of organic peroxides include 1,3-bis(t-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexene-3, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, 2,2'-bis(t-butylperoxy)-p-isopropylbenzene, dicumyl peroxide, di-t-butyl peroxide, and t-butyl peroxide.
[0070] Examples of the phenol resin include p-substituted phenol compounds represented by the following formula (7), o-substituted phenol-aldehyde condensates, m-substituted phenol-aldehyde condensates, and brominated alkylphenol-aldehyde condensates. Among these, p-substituted phenol compounds are preferred. The p-substituted phenol compounds can be obtained by condensation reaction of p-substituted phenol with aldehyde (preferably formaldehyde) in the presence of an alkali catalyst. [ka] (In formula (7), X is a hydroxyl group, a halogenated alkyl group, or a halogen atom. R is a monovalent saturated hydrocarbon group having 1 to 15 carbon atoms. n is an integer of 0 to 10.)
[0071] Commercially available phenolic resins include "Tackirol 201" (alkylphenol formaldehyde resin, manufactured by Taoka Chemical Industry Co., Ltd.), "Tackirol 250-I" (brominated alkylphenol formaldehyde resin with a bromination rate of 4%, manufactured by Taoka Chemical Industry Co., Ltd.), "Tackirol 250-III" (brominated alkylphenol formaldehyde resin, manufactured by Taoka Chemical Industry Co., Ltd.), and "PR-4507" (group Examples of such resins include those manufactured by Sakae Chemical Industry Co., Ltd.), product name "ST137X" (manufactured by Rohm & Haas Co., Ltd.), product name "Sumilite Resin PR-22193" (manufactured by Sumitomo Durez Co., Ltd.), product name "Tamanol 531" (manufactured by Arakawa Chemical Industry Co., Ltd.), product name "SP1059", product name "SP1045", product name "SP1055", product name "SP1056" (all manufactured by Schenectady Co., Ltd.), and product name "CRM-0803" (manufactured by Showa Union Synthetic Co., Ltd.). Among these, "Tackirol 201" can be preferably used.
[0072] The amount of the crosslinking agent is preferably 0.01 to 20 parts by mass, more preferably 0.1 to 15 parts by mass, and even more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the total rubber components contained in the polymer composition.
[0073] Resin components The composition may further contain a resin component together with the rubber component. The type of the resin component is not particularly limited, but examples thereof include polyolefin resins such as polyethylene and polypropylene. When the composition contains a resin component, the amount of the resin component is preferably 1 to 50 parts by mass, more preferably 5 to 40 parts by mass, based on 100 parts by mass of the total amount of the rubber components contained in the polymer composition.
[0074] In addition to the above-mentioned components, the composition may contain various additives that are generally used in rubber compositions for obtaining vulcanized rubber for various applications such as tires, hoses, vibration-proofing, belts, etc. Examples of such additives include antioxidants, zinc oxide, stearic acid, softeners, sulfur, vulcanization accelerators, etc. The amount of each of these additives may be appropriately selected depending on the type of additive within a range that does not impair the effects of the present invention.
[0075] <Cross-linked body and tire> The crosslinked body of the present invention can be obtained by subjecting the above-mentioned polymer composition to a crosslinking treatment. When obtaining a rubber molded article as a crosslinked body, the polymer composition is usually molded into a predetermined shape and then crosslinked. The rubber molded article can be produced according to a conventional method. For example, a tire is produced by mixing the above-mentioned polymer composition in a mixer such as a roll or a mixer, molding the mixture into a predetermined shape, and disposing the mixture in a predetermined position according to a conventional method to perform vulcanization molding. This forms one or both of a tread and a sidewall, and a pneumatic tire can be obtained.
[0076] The vulcanized rubber, which is the crosslinked product of the present invention, has excellent mechanical strength and can be applied to various rubber molded products. Specifically, it can be used as a material for tire treads and sidewalls; rolls for industrial machines and facilities, anti-vibration rubbers; various hoses and hose covers such as diaphragms, radiator hoses, and air hoses; seals such as packings, gaskets, weather strips, O-rings, and oil seals; belts such as power transmission belts; linings, dust boots, wire harnesses, shoe soles, and the like. Among these, it is suitable as tire members, anti-vibration members, belt members, roll members, hose members, wire harness members, and shoe sole members, and is more suitable as tire members, anti-vibration members, roll members, and belt members.
[0077] Furthermore, the crosslinked product of the present invention exhibits high abrasion resistance and excellent grip performance on ice, and is therefore particularly suitable for tire components, and among tire components, is particularly suitable for winter tires and all-season tires, and is particularly suitable as a material for either or both of the tread and sidewall of tires. EXAMPLES
[0078] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. In the examples and comparative examples, "parts" and "%" are based on mass unless otherwise specified. The measurement methods for various physical properties are shown below.
[0079] [Bound styrene content (mass%)]: 400MHz 1 The carbon black was determined by H-NMR. [Vinyl content (mol%)]: 400MHz 1 The carbon black was determined by H-NMR. [Hydrogenation rate (%)] and [θ]: 500MHz 1 The carbon black was determined by H-NMR. [1st peak weight average molecular weight]: Calculated in polystyrene equivalent from the retention time corresponding to the apex of the maximum peak in a GPC curve obtained using a gel permeation chromatography (GPC) apparatus (HLC-8120GPC (product name (manufactured by Tosoh Corporation))). (GPC conditions) Column: Product name "GMHXL" (Tosoh Corporation) x 2 Column temperature: 40°C Mobile phase: Tetrahydrofuran Flow rate; 1.0ml / min Sample concentration: 10mg / 20ml [Total weight average molecular weight]: The total weight average molecular weight was calculated in terms of polystyrene from the GPC curve obtained under the above GPC conditions using a GPC apparatus (HLC-8120GPC (product name, manufactured by Tosoh Corporation)). [Glass transition temperature Tg (° C.)]: Measured by differential scanning calorimetry (DSC) in accordance with ASTM D3418.
[0080] <Production of hydrogenation catalyst> [Synthesis of catalyst E] A 1 L three-necked flask equipped with a stirrer and a dropping funnel was purged with dry nitrogen, and 200 ml of anhydrous tetrahydrofuran and 0.2 mol of tetrahydrofurfuryl alcohol were added. Then, n-butyllithium / cyclohexane solution (0.2 mol) was added dropwise to the three-necked flask at 15°C to carry out a reaction, and a tetrahydrofuran solution of tetrahydrofurfuryloxylithium was obtained. Next, a 1L three-neck flask equipped with a stirrer and a dropping funnel was replaced with dry nitrogen, and 49.8g (0.2 moles) of bis(η5-cyclopentadienyl)titanium dichloride and 250ml of anhydrous tetrahydrofuran were added. Then, the tetrahydrofuran solution of tetrafurfuryloxylithium obtained by the method described above was added dropwise at room temperature with stirring for about 1 hour. After about 2 hours, the reddish brown liquid was filtered, and the insoluble portion was washed with dichloromethane. The filtrate and the washings were then combined and the solvent was removed under reduced pressure to obtain catalyst E [bis(η5-cyclopentadienyl)titanium(tetrahydrofurfuryloxy)chloride] (also called "chlorobis(2,4-cyclopentadienyl)titanium(IV) tetrahydrofurfurylalkoxide"). The yield was 95%.
[0081] <Production of Conjugated Diene Polymer> [Production Example 1: Synthesis of Conjugated Diene Polymer A-1] A 50-liter autoclave reactor with nitrogen gas was charged with 25,900 g of cyclohexane, 26 g of tetrahydrofuran, 1,273 g of styrene, and 2,361 g of 1,3-butadiene. After adjusting the temperature of the reactor contents to 45°C, a cyclohexane solution containing n-butyllithium (39 mmol) was added to initiate polymerization. The polymerization was carried out under adiabatic conditions, and the maximum temperature reached 80°C. After confirming that the polymerization conversion rate had reached 99%, 111 g of butadiene was added and the polymerization was continued for another 5 minutes to obtain a reaction liquid containing a polymer. 2 mmol of silicon tetrachloride was added to the reaction liquid obtained and the reaction was continued for 10 minutes, and 28 mmol of N,N-dimethyl-3-(triethoxysilyl)propylamine was added and the reaction was continued for 20 minutes. Next, the reaction solution was heated to 80°C or higher and hydrogen was introduced into the system, after which 3.2 g of diethylaluminum chloride, 2.4 g of catalyst E, and n-butyllithium (15 mmol) were added, and hydrogen was supplied until a predetermined hydrogen accumulation value was reached while maintaining a hydrogen pressure of 0.7 MPa or higher to carry out the reaction. The reaction solution was then returned to room temperature and pressure and withdrawn from the reaction vessel to obtain a polymer solution. 1.4 g of 2,6-di-tert-butyl-p-cresol was added to the obtained polymer solution containing hydrogenated conjugated diene copolymer. Next, an aqueous solution (temperature: 80 ° C.) adjusted to pH 8.5 (pH at 80 ° C. by glass electrode method) with ammonia as a pH adjuster was placed in a desolvation tank, and the above polymer solution was further added (ratio of 1000 parts by mass of the above aqueous solution to 100 parts by mass of the polymer solution), and the solvent was removed by steam stripping (steam temperature: 190 ° C.) for 2 hours at a liquid phase temperature of 95 ° C. in the desolvation tank, and drying was performed with a heat roll adjusted to 110 ° C. to obtain a conjugated diene polymer A-1. The analytical values of the obtained conjugated diene polymer A-1 are shown in Table 2. The 1st peak weight average molecular weight of the obtained conjugated diene polymer A-1 was 20 × 10 4 , the weight average molecular weight (total weight average molecular weight) is 34 × 10 4 The hydrogenation rate was 93% (θ=0.93), and the glass transition temperature was -34°C.
[0082] [Production Examples 2 to 7, 9: Synthesis of Conjugated Diene Polymers A-2 to A-7, A-9] Conjugated diene polymers A-2 to A-7 and A-9 were obtained by polymerization in the same manner as in Production Example 1, except that the raw materials used were changed as shown in Table 1 and the hydrogenation time was changed. The analytical values of the conjugated diene polymers A-2 to A-7 and A-9 are shown in Table 2.
[0083] [Production Example 8: Synthesis of conjugated diene polymer A-8] A 50-liter autoclave reactor with nitrogen gas was charged with 25,900 g of cyclohexane, 26 g of tetrahydrofuran, 1,273 g of styrene, and 2,361 g of 1,3-butadiene. After adjusting the temperature of the reactor contents to 45°C, a cyclohexane solution containing n-butyllithium (39 mmol) was added to initiate polymerization. The polymerization was carried out under adiabatic conditions, and the maximum temperature reached 80°C. After confirming that the polymerization conversion rate reached 99%, 111 g of butadiene was added and polymerized for another 5 minutes to obtain a reaction solution containing a polymer. 2 mmol of silicon tetrachloride was added to the obtained reaction solution and reacted for 10 minutes, and 28 mmol of N,N-dimethyl-3-(triethoxysilyl)propylamine was added and reacted for 20 minutes. Next, the reaction solution was heated to 80°C or higher and hydrogen was introduced into the system, and the reaction solution was returned to room temperature and pressure and extracted from the reaction vessel to obtain a polymer solution. 1.4 g of 2,6-di-tert-butyl-p-cresol was added to the obtained polymer solution containing a conjugated diene copolymer. Next, an aqueous solution (temperature: 80 ° C.) adjusted to pH 8.5 (pH at 80 ° C. by glass electrode method) with ammonia, which is a pH adjuster, was placed in a desolvation tank, and the above polymer solution was further added (ratio of 1000 parts by mass of the above aqueous solution to 100 parts by mass of the polymer solution), and the solvent was removed by steam stripping (steam temperature: 190 ° C.) for 2 hours at a liquid phase temperature of 95 ° C. in the desolvation tank, and drying was performed with a heat roll adjusted to 110 ° C. to obtain a conjugated diene polymer A-8. The 1st peak weight average molecular weight of the obtained conjugated diene polymer A-8 was 20 × 10 4 , the weight average molecular weight (total weight average molecular weight) is 34 × 10 4 The glass transition temperature was −40° C. The conjugated diene polymer A-8 had a hydrogenation rate of 0% and an angle θ of 0.
[0084] [Table 1]
[0085] In Table 1, the abbreviations of the compounds represent the following compounds. Compound A: piperidine Compound B: N,N-dimethyl-3-(triethoxysilyl)propylamine Compound C: Silicon tetrachloride In Table 1, "-" indicates that the compound in the corresponding column was not used.
[0086] [Table 2]
[0087] <Production of polymer composition and evaluation of properties> [Examples 1 to 19 and Comparative Examples 1 to 4] In the first stage of kneading, a conjugated diene polymer, (B) water-soluble component, (C) porous particles, silica, silane coupling agent, extender oil, stearic acid, zinc oxide, and antioxidant were kneaded according to the formulations in Tables 3 and 4 at a filling rate of 72% and a rotation speed of 60 rpm using a plastomill (capacity 250 cc) equipped with a temperature control device. Then, in the second stage of kneading, the compound obtained above was cooled to room temperature, and then sulfur and a vulcanization accelerator were kneaded. This was molded and vulcanized in a vulcanization press at 160°C for a predetermined time. The following property evaluations (1) to (3) were carried out using the polymer composition, the rubber before vulcanization, and the vulcanized rubber. The types and blending ratios of the conjugated diene-based polymer, the water-soluble component (B), and the porous particles (C) used in each Example and Comparative Example are as shown in Tables 3 and 4. The values in Tables 3 and 4 represent the blending ratio (parts by mass) of each component. In Comparative Examples 1 and 2, the water-soluble component (B) was not blended. In Examples 16 to 19, the porous particles (C) were blended.
[0088] <Characteristics evaluation> (1) Abrasion resistance Using vulcanized rubber as a measurement sample, a DIN abrasion tester (manufactured by Toyo Seiki Co., Ltd.) was used, and measurements were made in accordance with JIS K 6264-2:2005 under a load of 10 N at 25° C. The abrasion resistance was expressed as an index with Comparative Example 2 set at 100, and a larger value indicates better abrasion resistance. (2) Grip performance on ice The frictional force generated when a vulcanized rubber with a diameter of 50 mm and a thickness of 10 mm was pressed against a fixed piece of ice and rotated was detected by a load cell, and the dynamic friction coefficient μ was calculated. The measurement temperature was -2°C and the surface pressure was 12 kgf / cm 2 The sample rotation peripheral speed was 20 cm / sec. The coefficient of dynamic friction μ of Comparative Example 2 is expressed as an index of 100, and a larger value indicates a larger coefficient of dynamic friction μ and better performance on ice. (3) Hardness (Duro-A hardness) The hardness (Duro-A hardness) of each test piece made of each vulcanized rubber sheet before and after heat aging was measured in accordance with JIS K6253. The hardness was evaluated on a three-level scale, with a difference in hardness before and after heat aging of less than 3 being "A," a difference of 3 to less than 6 being "B," and a difference of 6 or more being "C." Note that "heat aging" here refers to the process of performing heat aging (100°C, 70 hours) on new vulcanized rubber in accordance with JIS K6257:2010 to obtain heat-aged vulcanized rubber.
[0089] The results of the characteristic evaluation of Examples 1 to 19 and Comparative Examples 1 to 4 are shown in Tables 3 and 4. [Table 3]
[0090] [Table 4]
[0091] In Tables 3 and 4, details of (B) the water-soluble component and (C) the porous particles are as follows. B-1: Magnesium sulfate, product name "MN-00", manufactured by Mai Chemical Industry Co., Ltd. B-2: Potassium sulfate, product name "KSO", manufactured by Ueno Pharmaceutical Co., Ltd. B-3: Sodium lignosulfonate, manufactured by Tokyo Chemical Industry Co., Ltd. B-4: Polyvinyl alcohol short fiber, product name "Kuralon 1239", manufactured by Kuraray Co., Ltd. B-5: Xanthan gum, product name "Rhodopol 23", manufactured by Rhodia B-6: Guar gum, product name "Emmulcoll 200 SP", manufactured by Degussa B-7: β-cyclodextrin, product name "Celdex B-100", manufactured by Nihon Shokuhin Kako Co., Ltd. C-1: Molecular sieve, product name "MS4A Powder", manufactured by Union Showa Co., Ltd. C-2: Porous cellulose particles, product name "Viscopearl Mini (particle size: 700 μm)", manufactured by Rengo Co., Ltd. C-3: Porous natural glass, product name "Permis LHM-90", manufactured by Hess C-4: Porous nylon particles, product name "Nylon 6 porous microparticles (average particle size: 13 μm)", manufactured by Toray Industries, Inc.
[0092] Details of the components *1) to *7) used in Tables 3 and 4 are as follows: *1) ZEOSIL 1165MP manufactured by Rhodia *2) Mitsubishi Chemical Diablack N339 *3) Evonik Si75 *4) JX Nippon Oil & Energy Corporation process oil T-DAE *5) Seiko Chemical Ozonone 6C *6) Noccela CZ manufactured by Ouchi Shinko Chemical Industry Co., Ltd. *7) Noccela D manufactured by Ouchi Shinko Chemical Industry Co., Ltd. In Tables 3 and 4, the numbers in parentheses indicate the blending amount (parts by mass) of each component when the polymer composition was prepared. "-" indicates that the compound in the corresponding column was not used.
[0093] As shown in Tables 3 and 4, in the polymer compositions (Examples 1 to 19) containing the conjugated diene polymer (A) having a hydrogenation rate of 75% or more and the water-soluble component (B), the abrasion resistance and grip performance on ice were improved in a well-balanced manner compared to Comparative Examples 1 to 4. In addition, the vulcanized rubber obtained using the polymer compositions of Examples 1 to 19 showed a small increase in hardness due to heat aging. From these results, it was found that the rubber compositions of Examples 1 to 19, which contain the polymer (A) and the water-soluble component (B), can produce vulcanized rubber that exhibits good grip performance on ice, has excellent abrasion resistance, and suppresses the increase in hardness due to heat aging. In addition, the incorporation of the porous particles (C) further improved the grip performance on ice of the vulcanized rubber.
[0094] From the above results, it was found that the polymer composition containing the polymer (A) and the water-soluble component (B) can improve the abrasion resistance while maintaining high grip performance on ice. It was also found that the polymer composition containing the polymer (A) and the water-soluble component (B) can suppress the increase in hardness due to heat aging.
Claims
1. (A) a conjugated diene-based polymer having a carbon-carbon unsaturated bond, in which the value θ represented by the following formula (i) is 0.75 or more, where p, q, r and s are the constituent ratios (molar ratios) in the polymer of a structural unit represented by the following formula (1), a structural unit represented by the following formula (2), a structural unit represented by the following formula (3), and a structural unit represented by the following formula (4), respectively; (B) at least one component selected from the group consisting of water-soluble particles and water-soluble fibers; A polymer composition comprising: Formula (i): θ=(p+(0.5×r)) / (p+q+(0.5×r)+s) [Formula 1]
2. The polymer composition according to claim 1, wherein the conjugated diene polymer (A) has at least one functional group selected from the group consisting of an amino group, a nitrogen-containing heterocyclic group, a phosphino group, a hydroxyl group, a thiol group, and a hydrocarbyloxysilyl group.
3. 3. The polymer composition according to claim 1, wherein the conjugated diene polymer (A) has a partial structure derived from at least one compound selected from the group consisting of a compound represented by the following formula (5) and a compound represented by the following formula (6): [chemical 2] (In formula (5), A 1 has at least one atom selected from the group consisting of nitrogen, phosphorus, oxygen, sulfur and silicon, has no active hydrogen, and R 5 R is a monovalent functional group bonded to a nitrogen atom, a phosphorus atom, an oxygen atom, a sulfur atom, a silicon atom, or a carbon atom contained in a carbonyl group, or is a (thio)epoxy group. 3 and R 4 are each independently a hydrocarbyl group. 5 is a hydrocarbylene group. r is an integer from 0 to 2. However, when r is 2, multiple R 3 are the same or different groups. When r is 0 or 1, multiple R 4 are the same or different groups.) [C3] (In formula (6), A 2 has at least one atom selected from the group consisting of nitrogen, phosphorus, oxygen, sulfur and silicon, has no active hydrogen, and R 9 R is a monovalent functional group bonded to R via a nitrogen atom, phosphorus atom, oxygen atom, sulfur atom, or silicon atom, or a hydrocarbyl group having 1 to 20 carbon atoms. 6 and R 7 are each independently a hydrocarbyl group. 8 is a hydrocarbylene group. 9 is a single bond or a hydrocarbylene group. m is 0 or 1. However, when m is 0, multiple R 7 are the same or different groups.)
4. The polymer composition according to any one of claims 1 to 3, wherein the glass transition temperature of the conjugated diene polymer (A) is -40°C or lower.
5. The weight average molecular weight (Mw) of the conjugated diene polymer (A) measured by gel permeation chromatography in terms of polystyrene is 1.0×10 5 ~2.0 x 10 6 The polymer composition according to any one of claims 1 to 4,
6. The polymer composition according to any one of claims 1 to 5, wherein the content of the component (B) is 0.1 to 40 parts by mass based on 100 parts by mass of the conjugated diene polymer (A).
7. The polymer composition according to any one of claims 1 to 6, further comprising porous particles.
8. The polymer composition according to any one of claims 1 to 7, further comprising a crosslinking agent.
9. The polymer composition according to any one of claims 1 to 8, further comprising at least one selected from the group consisting of silica and carbon black.
10. A crosslinked product obtained by using the polymer composition according to any one of claims 1 to 9.
11. A tire having a tread and / or a sidewall formed from the polymer composition according to any one of claims 1 to 9.
Citation Information
Patent Citations
Tire for iced and snowy road
JP1990077305A
Tread having a composition containing guar gum powder
JP2010514867A
Winter tires with improved grip on ice
JP2013514399A
Rubber composition for winter tire treads
JP2013522427A
Rubber composition for studless tire
JP2017095560A