Secondary battery, battery module, battery pack and power consuming device
By adjusting Co and Al content in the positive electrode material and using a specific electrolyte compound, the oxidative decomposition reactions at the positive electrode interface are mitigated, reducing self-discharge and impedance, and enhancing the discharge capacity and cycle stability of secondary batteries.
Patent Information
- Application Number
- JP2022553657
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-09-27
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-09-27
AI Technical Summary
Conventional secondary batteries, particularly lithium ion secondary batteries, experience accelerated decay due to oxidative decomposition reactions at the positive electrode interface when stored in a high state of charge (SOC), leading to increased self-discharge rates and impedance, which shortens their service life and limits their performance.
Adjusting the content of Co and Al elements in the positive electrode material and incorporating a specific compound in the electrolyte, represented by general formula (I), to form a chelate structure that stabilizes the positive electrode surface and separates the electrolyte interface, reducing side reactions and improving structural stability and ionic conductivity.
This approach effectively reduces self-discharge rates, decreases storage impedance, and enhances discharge capacity efficiency by stabilizing the positive electrode material, thereby extending the battery's service life and improving its cycle performance.
Smart Images

Figure 0007569482000023 
Figure 0007569482000024 
Figure 0007569482000025
Abstract
Description
[Technical field]
[0001] The present application relates to the technical field of secondary batteries, and in particular to secondary batteries, battery modules, battery packs and power consuming devices. [Background technology]
[0002] In recent years, as the application range of secondary batteries expands, secondary batteries are widely used in various fields such as energy storage power systems such as hydroelectric, thermal, wind, and solar power stations, as well as electric tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace, etc. As secondary batteries have undergone great development and the demand is huge, the requirements for their energy density, cycle performance, safety performance, etc. are also increasing, and improvement in cost performance is expected.
[0003] In addition, in secondary batteries, particularly lithium-ion secondary batteries, when stored while charged, the positive electrode is in a high SOC state, and the interfacial oxidation activity between the positive electrode and the solvent is very high. After the solvent comes into contact with the positive electrode interface, an oxidative decomposition reaction occurs, making the structure of the positive electrode material unstable and reducing the ability and speed of lithium intercalation and deintercalation. Furthermore, self-discharge within the secondary battery cell continues, accelerating the attenuation of the service life of the secondary battery, and the gas generated at the interface due to the reaction between the solvent and the positive electrode interface leads to an increase in the impedance of the positive electrode interface, etc.
[0004] In the prior art, the cathode material is generally doped or coated in various ways to physically separate the electrolyte and the cathode interface to obtain a stable cathode structure, but in these techniques, the coating layer is fragile, and when broken, the interface reaction continues to occur, causing serious self-discharge of the cell and a rapid shortening of the battery life; or the amount of the material to be doped or coated is small, resulting in insufficient protection, limiting the improvement of battery performance; or the amount of the material to be doped or coated is sufficient to form a stable interface protective film, but the protective film seriously deteriorates the interface impedance. Therefore, there is room for improvement in the conventional processing technology of the cathode material. Summary of the Invention [Problem to be solved by the invention]
[0005] The present application has been made in consideration of the above technical problems, and aims to provide a secondary battery that reduces the cost of a secondary battery, effectively reduces the self-discharge rate of a cell, improves the rate of increase in the cell's storage impedance, and has excellent rate discharge capacity efficiency. [Means for solving the problem]
[0006] In order to achieve the above object, the inventors of the present application have conducted intensive research and have found that the above technical problems can be solved by adjusting specific metal elements in the positive electrode material of a secondary battery and using specific additives in the electrolyte.
[0007] The first aspect of the present application is The battery includes a positive electrode plate, a negative electrode plate, and an electrolyte solution, The positive plate includes a positive active material; In the positive electrode active material, the content of Co element satisfies Co≦0.09, and the content of Al element satisfies 500 ppm≦Al≦10000 ppm; The electrolyte solution contains a compound represented by the following general formula (I): [ka] In the general formula (I), A 1 ~A 4 are each independently a single bond or an alkylene group having 1 to 5 carbon atoms; R 1 , R 1 ' are each independently [ka] and R 2 teeth, [ka] and R 3 is an alkylene group or an alkyleneoxy group having 1 to 3 carbon atoms.
[0008] Therefore, in the present application, by reducing the Co content in the positive electrode active material, the cost of the positive electrode material can be reduced; by including Al in the positive electrode active material and appropriately adjusting the Al content, the degree of Li / Ni mixing caused by the reduction of the Co content can be reduced, and the structural stability and ionic conductivity of the positive electrode material can be improved; and by including the compound represented by the above general formula (I) in the electrolyte, the compound represented by the general formula (I) forms a chelate compound with Al, thereby effectively stabilizing the Al element on the surface of the positive electrode material, and separating the electrolyte and the positive electrode interface, thereby reducing side reactions at the interface, thereby reducing the cost of the secondary battery, effectively reducing the self-discharge rate of the cell, improving the increase rate of the cell storage impedance, and obtaining a secondary battery that improves the capacity efficiency of rate discharge.
[0009] In any embodiment, the concentration of the compound of general formula (I) in the electrolyte solution is 0.01% by mass to 15% by mass, preferably 0.1% by mass to 10% by mass, and more preferably 0.5% by mass to 5% by mass.
[0010] Therefore, it is possible to achieve a balance between a reduction in the self-discharge rate of the secondary battery, a reduction in the rate of increase in the storage impedance of the cell, and an improvement in the capacity efficiency of the rate discharge.
[0011] In any embodiment, preferably, in the general formula (I), A 1 ~A 4 are each independently a single bond or an alkylene group having 1 to 3 carbon atoms, and may further be a single bond or a methylene group. 2 teeth, [ka] and R 3 is an alkylene group or alkyleneoxy group having 1 or 2 carbon atoms.
[0012] Therefore, the compound represented by general formula (I) can form a chelate compound with Al to effectively stabilize the surface of the positive electrode material and separate the electrolyte and positive electrode interface, thereby effectively reducing the self-discharge rate of the cell, improving the increase rate of the cell's storage impedance, and improving the capacity efficiency of the battery's rate discharge.
[0013] In addition, in any embodiment, the compound represented by the general formula (I) is at least one selected from the following compounds 1-18.
[0014] [ka]
[0015] Therefore, it is possible to further stabilize the surface of the positive electrode material, reduce the self-discharge rate of the cell, improve the increase rate of the storage impedance of the cell, and improve the capacity efficiency of the rate discharge.
[0016] In any embodiment, the content of Al element preferably satisfies 1000 ppm≦Al≦10000 ppm, and more preferably satisfies 1000 ppm≦Al≦7000 ppm.
[0017] Therefore, it is possible to further reduce the self-discharge rate of the cell, improve the increase rate of the storage impedance of the cell, and improve the capacity efficiency of the rate discharge.
[0018] Also, in any embodiment, the general formula of the positive electrode active material is LiNi z Mn y Co x Al a O 2 where x ≦ 0.09, 0.0005 ≦ a ≦ 0.01, 0.5 < z < 1, 0 < y < 0.4, and x + y + z + a = 1. Therefore, it is possible to simultaneously achieve a reduction in the cost of the secondary battery and an improvement in the structural stability and ionic conductivity of the positive electrode material.
[0019] In any embodiment, preferably, the electrolytic solution further contains at least one other additive selected from lithium tetrafluoroborate, lithium bis(oxalato)borate, lithium difluoro(oxalato)borate, and tris(trimethylsilyl)borate. Preferably, the concentration of the total amount of the other additive in the electrolytic solution is 0.2% by mass to 3% by mass. Therefore, it is possible to further reduce the self-discharge rate of the cell, improve the increase rate of the storage impedance of the cell, and improve the capacity efficiency of the rate discharge.
[0020] In any embodiment, preferably, the specific surface area of the positive electrode active material is 0.5 to 3 m 2 / g, and more preferably 0.5 to 2.5 m 2 / g. In this way, it is possible to achieve high-speed transport of lithium ions and suppress side reactions on the positive electrode surface, and meet the needs of high-speed charge and discharge of the cell.
[0021] The second aspect of the present application further provides a battery module including the secondary battery of the first aspect of the present application. The third aspect of the present application further provides a battery pack including the battery module of the second aspect of the present application. The fourth aspect of the present application further provides a power consumption device including the secondary battery of the first aspect of the present application, the battery module of the second aspect, or the battery pack of the third aspect.
[0022] The battery module, battery pack and power consuming device of the present application include the secondary battery of the first aspect of the present application, and therefore have at least the same or similar technical effects as the secondary battery. [Brief description of the drawings]
[0023] [Figure 1] FIG. 1 is a schematic diagram of a secondary battery according to an embodiment of the present application. [Diagram 2] FIG. 2 is an exploded view of the secondary battery according to the embodiment of the present application shown in FIG. [Diagram 3] FIG. 1 is a schematic diagram of a battery module according to an embodiment of the present application. [Figure 4] FIG. 1 is a schematic diagram of a battery pack according to an embodiment of the present application. [Diagram 5] FIG. 5 is an exploded view of the battery pack according to the embodiment of the present application shown in FIG. 4. [Figure 6] 1 is a schematic diagram of a power consuming device according to an embodiment of the present application; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] Hereinafter, the secondary battery, battery module, battery pack, and power consumption An embodiment specifically disclosing the device will be described in detail. However, unnecessary detailed description may be omitted. For example, detailed description of known matters and repeated description of substantially the same structure may be omitted. This is to avoid the following description from becoming unnecessarily long and to make it easy for those skilled in the art to understand. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.
[0025] The "ranges" disclosed herein are defined in the form of lower and upper limits, and a given range is defined by selecting one lower limit and one upper limit, with the selected lower and upper limits defining the boundaries of the particular range. The ranges thus defined may or may not include the endpoint values and may be arbitrarily combined, i.e., any lower limit and any upper limit may be combined to form a range. For example, if ranges of 60-120 and 80-110 are listed for a particular parameter, it is understood that the ranges of 60-110 and 80-120 are also contemplated. Also, if 1 and 2 are listed as the minimum range values and 3, 4, and 5 are listed as the maximum range values, all of the ranges of 1-3, 1-4, 1-5, 2-3, 2-4, and 2-5 are contemplated. In this application, unless otherwise specified, the numerical range "a-b" represents a shorthand notation for any combination of real numbers between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed herein, with "0-5" being merely a shorthand for combinations of these numbers. Also, when a parameter is described as an integer ≧2, this is equivalent to disclosing that the parameter is, for example, the integers 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0026] Unless otherwise specified, all and any embodiments of the present application can be combined with each other to form a new technical solution. Unless otherwise specified, all and any technical features of the present application can be combined with each other to form a new technical solution.
[0027] Unless otherwise specified, all steps in the present application may be performed in sequence or randomly, preferably in sequence. For example, the method includes steps (a) and (b) indicating that the method may include steps (a) and (b) performed in sequence, or may include steps (b) and (a) performed in sequence. For example, the method may further include step (c) indicating that step (c) can be added to the method in any order, for example, the method may include steps (a), (b) and (c), may include steps (a), (c) and (b), may include steps (c), (a) and (b), etc.
[0028] Unless otherwise specified, the terms "comprise" and "inclusion" in this application may be open or closed. For example, the terms "comprise" and "inclusion" may mean that the term further includes or includes other components not listed, or that the term only includes or includes the components listed.
[0029] In this application, unless otherwise specified, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B." More specifically, the condition A is true (or exists) and B is false (or does not exist), the condition A is false (or does not exist) and B is true (or exists), or the condition A and B are both true (or exist) all satisfy the condition "A or B."
[0030] In one embodiment of the present application, the present application provides a secondary battery, and as an example, the present application proposes a lithium-ion secondary battery.
[0031] [Secondary battery] The secondary battery of the present application includes a positive electrode plate, a negative electrode plate, and an electrolyte. The positive electrode plate includes a positive electrode active material, in which the content of Co element in the positive electrode active material satisfies Co≦0.09 and the content of Al element satisfies 500 ppm≦Al≦10000 ppm. In addition, the electrolyte includes a compound represented by the following general formula (I): [ka] In the general formula (I), A 1 ~A 4 are each independently a single bond or an alkylene group having 1 to 5 carbon atoms; R 1 , R 1 ' are each independently [ka] and R 2 teeth, [ka] and R 3 is an alkylene group or alkyleneoxy group having 1 to 3 carbon atoms.
[0032] The applicant unexpectedly discovered that by reducing the content of Co element in the positive electrode active material of a secondary battery, containing an appropriate amount of Al element, and further containing a compound represented by general formula (I) in the electrolyte, it is possible to reduce the cost of the secondary battery, effectively reduce the self-discharge rate of the cell, improve the increase rate of the cell storage impedance, and obtain a secondary battery with excellent rate discharge capacity efficiency.
[0033] Although the mechanism is not yet clear, the applicant believes as follows. In the composition of secondary batteries, the cost of the positive electrode material is the highest. Take lithium-ion secondary batteries as an example, the price of cobalt element in the ternary positive electrode is the highest and fluctuates greatly, and there is a shortage of resources, so reducing the content of cobalt element can significantly reduce the cost of secondary batteries. On the other hand, reducing the content of cobalt element not only reduces the electronic conductivity of the ternary positive electrode material, but also increases Li / Ni mixing, restricts the solid-phase migration and diffusion of lithium ions, and reduces the ion transport performance of the positive electrode material. In addition, Li / Ni mixing causes irreversible phase transition of the positive electrode material, promotes the crushing of the positive electrode particles, and exposes many new surfaces, which results in the side reaction between the positive electrode active material and the electrolyte continuing to occur at the interface between the positive electrode material and the electrolyte, causing the self-discharge in the cell to continue and the impedance to increase significantly.
[0034] Therefore, by introducing Al element in the synthesis of the positive electrode active material and distributing the Al element uniformly in the bulk phase and on the surface, the degree of Li / Ni mixing can be effectively reduced, which not only improves the structural stability and ionic conductivity of the positive electrode material, but also makes the spherical morphology of the positive electrode material more uniform, which is favorable for releasing the stress caused by the structural change of the positive electrode material during lithium intercalation and deintercalation, and further improves the structural stability of the positive electrode material.
[0035] However, due to the unstable bond unsaturated structure on the surface of the positive electrode material, the Al element on the surface is easily involved in the reaction during the charge and discharge process, and the effect of stabilizing the surface of the material cannot be obtained. By adding the compound represented by the above general formula (I) as an additive to the electrolyte, during the first charge, the compound is bonded to the Al on the surface of the positive electrode in a certain direction to form a chelate structure, and the two rings are opened and connected to each other to form a three-dimensional network structure, which is covered on the surface of the positive electrode particles, thereby effectively stabilizing the Al element on the surface of the positive electrode material and isolating the electrolyte and the positive electrode interface. In this way, not only can the stability and ion conductivity of the positive electrode surface structure be improved, but also the side reaction at the interface can be reduced, the self-discharge rate of the cell is greatly reduced, the increase rate of the storage impedance is reduced, and the cycle performance is stabilized.
[0036] The combination of the positive electrode active material and the electrolyte according to the present application is not limited to being applicable to one battery structure, but can also be applied when the shape of the battery exterior or the battery is changed according to other needs, or when the assembly method of the electrode assembly (e.g., stacking, winding, etc.) is changed.
[0037] [Positive plate] The positive plate includes a positive current collector and a positive material disposed on at least one surface of the positive current collector.
[0038] As an example, a positive electrode current collector has two opposing surfaces in the thickness direction of the positive electrode current collector, and a positive electrode material is disposed on either or both of the two opposing surfaces of the positive electrode current collector.
[0039] The positive electrode material of the present application includes a positive electrode active material, and the positive electrode active material is selected from materials capable of intercalating and deintercalating lithium ions. Specifically, the positive electrode active material may be one or more selected from lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, other cobalt-containing oxide positive electrodes, composite positive electrodes consisting of the above compounds and lithium iron phosphate, lithium iron manganese phosphate, lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, etc., and compounds obtained by adding other transition metals or non-transition metals to the above compounds, but the present invention is not limited to these materials.
[0040] In the positive electrode active material of the present application, the content of Co element satisfies Co≦0.09. Therefore, by reducing the content of Co, which is the most expensive in the ternary positive electrode material, the cost of the secondary battery can be reduced and the cost performance of the secondary battery can be improved. However, when the Co element is reduced, the electronic conductivity of the ternary positive electrode material decreases, the Li / Ni mixing phenomenon increases, the ion transport performance of the positive electrode material decreases, and even causes the irreversible phase transition of the positive electrode material, which worsens the fracture of the positive electrode particles and exposes many new surfaces, resulting in the side reaction between the positive electrode active material and the electrolyte at the interface between the positive electrode material and the electrolyte, which causes the self-discharge in the cell to continue and the impedance to increase significantly.
[0041] For this reason, the positive electrode active material of the present application contains Al element, and the content of Al element satisfies 500ppm≦Al≦10000ppm. By controlling the uniform distribution of Al element in the bulk phase and on the surface of the positive electrode active material, the degree of Li / Ni mixing caused by the reduction of Co element can be effectively reduced, and the structural stability and ionic conductivity of the positive electrode material can be improved, and the spherical morphology of the positive electrode material can be made more uniform, which is favorable for stress release due to structural changes of the positive electrode material during the lithium intercalation / deintercalation process, and further improves the structural stability of the positive electrode material.
[0042] Furthermore, during the initial charge, the Al element on the surface of the positive electrode active material reacts with the compound represented by the above general formula (I) contained in the electrolyte to form a chelate structure, thereby stabilizing the Al element on the surface of the positive electrode active material, and the formed chelate compound can separate the interface between the electrolyte and the positive electrode material, thereby further stabilizing the positive electrode material, reducing side reactions at the interface, greatly reducing the self-discharge rate of the cell, reducing the increase rate of the storage impedance, improving the cycle stability, and extending the service life of the battery.
[0043] In some embodiments, in the positive electrode active material, the content of Al element satisfies 1000 ppm ≤ Al ≤ 10000 ppm, and preferably satisfies 1000 ppm ≤ Al ≤ 7000 ppm. Therefore, the structural stability of the positive electrode material can be further improved, the self-discharge rate of the cell can be reduced, the increase rate of the storage impedance can be decreased, the cycle stability can be improved, and the service life of the battery can be extended.
[0044] In some embodiments, the general formula of the positive electrode active material is LiNi z Mn y Co x Al a O 2 where x ≤ 0.09, 0.0005 ≤ a ≤ 0.01, 0.5 < z < 1, 0 < y < 0.4, and x + y + z + a = 1. Therefore, a positive electrode active material with a stable structure can be obtained, the self-discharge rate of the cell can be reduced, the increase rate of the storage impedance can be decreased, the cycle stability can be improved, and the service life of the battery can be extended.
[0045] In some embodiments, the specific surface area of the positive electrode active material is 0.5 - 3 m 2 / g, and preferably 1 - 2.5 m 2 / g. If the specific surface area of the positive electrode active material is too small and the reaction sites are insufficient, the transport of lithium ions at the interface will be slow. If the specific surface area is too large, side reactions will increase and the transport distance of lithium ions at the interface will be long, which will appear as an increase in the charge transfer resistance (Rct). By controlling the specific surface area of the positive electrode active material to 0.5 - 3 m 2 / g, not only can the side reactions on the positive electrode surface be controlled and the influence on the lithium ion transport path and the interface impedance be reduced, but also sufficient active sites on the positive electrode surface can be ensured to meet the high-speed transport performance of lithium ions at the interface, and the needs of high-speed charging and discharging of the cell can be met.
[0046] In some embodiments, the positive electrode material preferably includes a conductive agent. However, the type of the conductive agent is not specifically limited, and those skilled in the art can select it according to actual needs. For example, the conductive agent used in the positive electrode material may be one or more selected from superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0047] In the secondary battery of the present application, the positive electrode current collector can be a metal foil sheet or a composite current collector. For example, aluminum foil can be used as the metal foil sheet. The composite current collector may include a polymeric material substrate layer and a metal layer formed on at least one surface of the polymeric material substrate layer. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymeric material substrate (e.g., substrate such as polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE)), but the present application does not limit the materials.
[0048] In the present application, the positive electrode plate can be manufactured by a method known in the art. For example, the positive electrode material, conductive agent, and binder of the present application are dispersed in a solvent (e.g., N-methylpyrrolidone (NMP)) to form a uniform positive electrode slurry, and the positive electrode slurry is coated on a positive electrode current collector, followed by processes such as drying and cold pressing to obtain a positive electrode plate.
[0049] [Electrolyte] The electrolyte plays an ion conducting role between the positive and negative electrodes, and includes an organic solvent, a lithium salt, and an additive. In the present application, the electrolyte contains a compound represented by the following general formula (I) as an additive.
[0050] [ka]
[0051] In the general formula (I), A 1 ~A 4 are each independently a single bond or an alkylene group having 1 to 5 carbon atoms, preferably a single bond or an alkylene group having 1 to 3 carbon atoms, preferably a single bond or a methylene group; R 1 , R 1 ' are each independently [ka] and R 2 teeth, [ka] and R 3 is an alkylene group or an alkyleneoxy group having 1 to 3 carbon atoms, preferably an alkylene group or an alkyleneoxy group having 1 or 2 carbon atoms.
[0052] By using the compound represented by the above general formula (I) as an additive in the electrolyte, the compound is bonded to Al on the surface of the positive electrode in a predetermined direction during the initial charge to form a chelate structure, and the two rings of the compound are opened and connected to each other to form a three-dimensional mesh structure, which is covered on the surface of the positive electrode particles. This effectively stabilizes the Al element on the surface of the positive electrode material and separates the electrolyte from the positive electrode interface, thereby not only improving the stability and ionic conductivity of the positive electrode surface structure, but also reducing side reactions at the interface, greatly reducing the self-discharge rate of the cell, reducing the increase rate of storage impedance, improving the battery cycle stability, and improving the capacity efficiency of rate discharge.
[0053] In some embodiments, the compound represented by general formula (I) is at least one selected from the following compounds 1 to 18.
[0054] [ka]
[0055] Therefore, the stability of the positive electrode surface structure can be more effectively improved, the self-discharge rate of the cell can be reduced, the increase rate of the storage impedance can be decreased, and the capacity efficiency of the rate discharge can be improved.
[0056] In any embodiment, the percentage of the compound represented by general formula (I) in the electrolyte is 0.01% by mass to 15% by mass, preferably 0.1% by mass to 10% by mass, more preferably 0.5% by mass to 5% by mass. By controlling the content range of the compound represented by general formula (I) within the above range, the introduction of the compound represented by general formula (I) can stabilize Al on the positive electrode surface, and Al can suppress Li / Ni mixing, stabilize the positive electrode material structure, and improve ion conductivity. In addition, the chelation of the compound represented by general formula (I) with Al makes the compound uniformly distributed on the surface of the positive electrode, and the ring-opening crosslinking of the compound itself forms a network structure, which further protects the positive electrode interface and reduces side reactions at the interface.
[0057] The organic solvent contained in the electrolyte of the present application can be selected according to actual needs, and specifically, may contain one or more of chain carbonate esters, cyclic carbonates, and carboxylate esters. Among these, the type of chain carbonate esters, cyclic carbonates, and carboxylate esters is not particularly limited, and can be selected according to actual needs. Preferably, the organic solvent in the electrolyte is diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, vinyl carbonate, propylene carbonate, butylene carbonate, γ-butyrolactone, methyl formate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate. , Te It may also include one or more of tetrahydrofuran.
[0058] The organic solvent contained in the electrolyte of the present application may be selected according to actual needs, and specifically, may include one or more of chain carbonate esters, cyclic carbonates, and carboxylate esters. Of these, the types of chain carbonate esters, cyclic carbonates, and carboxylate esters are not particularly limited, and may be selected according to actual needs. Preferably, the organic solvent in the electrolyte may include one or more of diethyl carbonate, dipropyl carbonate, methyl ethyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, vinyl carbonate, propylene carbonate, butylene carbonate, γ-butyrolactone, methyl formate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, methyl propionate, and tetrahydrofuran.
[0059] In some embodiments, the electrolyte of the present application may further include at least one selected from unsaturated bond-containing cyclic carbonate compounds, halogen-substituted cyclic carbonate compounds, sulfite ester compounds, sultone compounds, disulfonic acid compounds, nitrile compounds, aromatic compounds, isocyanate compounds, phosphazene compounds, cyclic acid anhydride compounds, phosphite ester compounds, phosphate ester compounds, borate ester compounds, and carboxylate ester compounds as other additives. This can further improve the performance of the secondary battery, for example, further reduce the self-discharge rate of the secondary battery, and reduce the increase rate of storage impedance, etc.
[0060] [Negative plate] In the secondary battery of the present application, the negative electrode plate may include a negative electrode current collector and a negative electrode material layer disposed on the negative electrode current collector and containing a negative electrode active material, and the negative electrode material layer may be disposed on one side of the negative electrode current collector or on both sides of the negative electrode current collector. The type of the negative electrode active material is not specifically limited, and may be one or more selected from graphite, soft carbon, hard carbon, mesocarbon microspheres, carbon fiber, carbon nanotubes, silicon element, silicon oxide, silicon carbon composite material, and lithium titanate.
[0061] The negative electrode material layer of the present application may include a conductive agent, a binder, and any other auxiliary agent, and the type and content of the conductive agent and the binder are not specifically limited and may be selected according to actual needs. The negative electrode material layer is usually formed by coating a negative electrode slurry and drying it. The negative electrode slurry is usually formed by dispersing a negative electrode active material, any conductive agent, a binder, etc. in a solvent and stirring uniformly. The solvent may be N-methylpyrrolidone (NMP) or deionized water. As an example, the conductive agent may be one or more selected from superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers. As an example, the binder may be one or more selected from styrene butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS). Other optional auxiliaries are, for example, thickeners, such as sodium carboxymethylcellulose (CMC-Na).
[0062] The type of the negative electrode current collector is not specifically limited and can be selected according to actual needs. The negative electrode current collector can be a metal foil sheet or a composite current collector. For example, the metal foil sheet can be a copper foil. The composite current collector can include a polymeric material substrate layer and a metal layer formed on at least one surface of the polymeric material substrate. The composite current collector can be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, silver alloy, etc.) on a polymeric material substrate (e.g., a substrate such as polypropylene, polyethylene terephthalate, polybutylene terephthalate, polystyrene, polyethylene, etc.).
[0063] [Separator] Secondary batteries using an electrolyte solution and some secondary batteries using a solid electrolyte further include a separator. The separator is interposed between the positive and negative electrodes and plays a role in separation. The present application does not particularly limit the type of separator, and any well-known porous structure separator having good chemical and mechanical stability may be used. In some embodiments, the material of the separator may be one or more selected from glass fiber, nonwoven fabric, polyethylene, polypropylene, and polyvinylidene fluoride. The separator may be a single layer film or a multilayer composite film, and is not particularly limited. When the separator is a multilayer composite film, the materials of each layer may be the same or different, and are not particularly limited.
[0064] In some embodiments, the positive plates, negative plates, and separators may be configured into an electrode assembly by a winding or stacking process.
[0065] In some embodiments, the secondary battery may include an exterior body that packages the electrode assembly and the electrolyte.
[0066] In some embodiments, the exterior body of the secondary battery may be a hard case such as a hard plastic case, an aluminum case, a steel case, etc. The exterior body of the secondary battery may be a bag-type soft bag, etc. The material of the soft bag may be plastic, and examples of the plastic include polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).
[0067] In the present application, the shape of the secondary battery is not particularly limited, and it may be cylindrical, rectangular, or any other shape. For example, Fig. 1 shows a secondary battery 5 having a rectangular structure as an example.
[0068] In some embodiments, referring to FIG. 2, the exterior body may include a housing 51 and a top cover unit 53. The housing 51 may include a bottom plate and a side plate connected to the bottom plate, where the bottom plate and the side plate define a receiving cavity. The housing 51 has an opening communicating with the receiving cavity, and the top cover unit 53 covers the opening so as to seal the receiving cavity. The positive electrode plate, the negative electrode plate and the separator may be configured into an electrode assembly 52 by a winding process or a stacking process. The electrode assembly 52 is packaged in the receiving cavity. An electrolyte is impregnated into the electrode assembly 52. The number of electrode assemblies 52 included in the secondary battery 5 may be one or more, and can be selected by those skilled in the art according to specific practical needs.
[0069] The secondary battery, battery module, and battery pack of the present application will be described below with appropriate reference to the drawings.
[0070] [Battery module] In some embodiments, the secondary batteries may be assembled into a battery module, and the number of secondary batteries included in the battery module may be one or more, with the specific number being selectable by one skilled in the art based on the application and capacity of the battery module.
[0071] Fig. 3 shows an example of a battery module 4. Referring to Fig. 3, in the battery module 4, the secondary batteries 5 may be arranged in sequence along the length of the battery module 4. Of course, they may also be arranged in any other manner. Furthermore, the secondary batteries 5 may be fixed by fasteners.
[0072] Preferably, the battery module 4 may further include a casing having a storage space, and the multiple secondary batteries 5 are housed in the storage space.
[0073] [Battery pack] In some embodiments, the battery modules may also be assembled into a battery pack, and the number of battery modules included in the battery pack can be selected by those skilled in the art according to the application and capacity of the battery pack.
[0074] 4 and 5 show an example of a battery pack 1. Referring to Fig. 4 and Fig. 5, the battery pack 1 may include a battery housing and a plurality of battery modules 4 installed in the battery housing. The battery housing includes an upper housing 2 and a lower housing 3, and the upper housing 2 is covered by the lower housing 3 and forms a sealed space for accommodating the battery modules 4. The plurality of battery modules 4 are arranged in the battery housing in any manner.
[0075] [Power consumption equipment] The present application also provides a power consuming device, which includes one or more of the secondary batteries, battery modules, or battery packs provided by the present application. The secondary batteries, battery modules, or battery packs provided by the present application may function as a power source for the device, or as an energy storage unit for the device. The power consuming device of the present application may be, but is not limited to, a mobile device (e.g., a mobile phone, a laptop, etc.), an electric vehicle (e.g., a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), a train, a ship, a satellite, an energy storage system, etc.
[0076] The power consumption device can be selected as a secondary battery, a battery module or a battery pack according to the usage needs.
[0077] An example of an apparatus is shown in Figure 6. The apparatus may be a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. To meet the need for high power and high energy density of the secondary battery of the apparatus, a battery pack or a battery module can be used.
[0078] Other example devices may be mobile phones, tablet computers, notebook computers, etc. Such devices usually need to be thin and lightweight, and can use secondary batteries as a power source. EXAMPLES
[0079] The present invention will be further described below with reference to examples. It should be noted that these examples are merely illustrative of the present invention and do not limit the scope of the present invention. If no specific techniques or conditions are described in the examples, they are carried out according to the techniques, conditions or product instructions described in the literature in this field. If no manufacturer is described for the reagents or equipment used, they are all ordinary products available commercially.
[0080] Examples 1 to 24 and Comparative Examples 1 to 6 The secondary batteries of Examples 1 to 24 and Comparative Examples 1 to 6 were manufactured by the following method.
[0081] (1) Manufacturing of positive electrodes The positive electrode active material, acetylene black as a conductive agent, and polyvinylidene fluoride (PVDF) as a binder were added to N-methylpyrrolidone (NMP) as a solvent in a weight ratio of 94:3:3, and mixed uniformly to obtain a positive electrode slurry. The positive electrode slurry was coated on aluminum foil as a positive electrode current collector, and then the positive electrode plate was obtained through processes such as drying, cold pressing, and cutting. The structural formula and element contents of the positive electrode active material are shown in Table 1.
[0082] (2) Manufacturing of negative electrodes Artificial graphite as the negative electrode active material, acetylene black as the conductive agent, styrene butadiene rubber (SBR) as the binder, and sodium carboxymethylcellulose (CMC) as the thickener were added to deionized water as the solvent in a weight ratio of 95:2:2:1, and mixed uniformly to obtain a negative electrode slurry. The negative electrode slurry was then coated onto copper foil as a negative electrode current collector, and the negative electrode plate was obtained by carrying out processes such as drying, cold pressing, and cutting.
[0083] (3) Electrolyte production Glove box with argon gas atmosphere (H 2 O<0.1ppm, O 2 <0.1ppm), EC / EMC was mixed uniformly in a volume ratio of 3 / 7 as the organic solvent, and 1mol / L LiPF 6 A lithium salt was added and dissolved in an organic solvent, and the type and amount of the compound represented by general formula (I) or other additives shown in Table 1 was added and stirred uniformly to obtain an electrolyte solution.
[0084] (4) Separator manufacturing A polypropylene film was used as the separator.
[0085] (5) Manufacture of secondary batteries The positive plate, separator, and negative plate were stacked in this order so that the separator was interposed between the positive plate and the negative plate, and then wound to form an electrode assembly. The electrode assembly was then placed in a battery case and dried, after which an electrolyte solution was injected, and a secondary battery was manufactured through processes such as formation and standing.
[0086] [Testing relevant parameters of cathode materials] 1) Testing the content of Al element Take 2 g of the dried positive electrode material powder from the positive electrode plate and immerse it in aqua regia (H 2 SO 4 :HNO 3 After completely dissolving, test in accordance with the standard EPA 6010D-2018. See Table 1 for specific values.
[0087] 2) Specific surface area S test Use a scraper to remove the positive electrode material from the positive plate, and test it according to standard GB / T 19587-2004. The specific values are shown in Table 1.
[0088] [Battery performance test] 1. Self-discharge rate test for secondary batteries At 25°C, the secondary battery was charged to 4.35V at a constant current of 0.33C, then charged to a constant voltage of 4.35V until the current was less than 0.05C, and discharged to 2.8V at a constant current of 0.33C. After one charge-discharge, the secondary battery was charged to 4.35V at a constant current of 0.33C, and then charged to a constant voltage of 4.35V until the current was less than 0.05C. After leaving it for 5 minutes, the initial voltage V1 (mV) was measured, and the secondary battery was left in a 60°C oven for 48 hours, then taken out and restored to room temperature, and the secondary battery voltage V2 (mV) was measured. The self-discharge rate K of the secondary battery was calculated as K = (V2 - V1) / 48 (unit: mV / h).
[0089] 2. Storage impedance increase rate test The secondary battery was charged to 4.35V at a constant current of 0.33C, and then charged at a constant voltage until the current became less than 0.05C. After leaving it for 5 minutes, the initial voltage V1 was measured. The secondary battery was discharged for 15 seconds at a current of 4C, and the voltage V3 after discharge was measured. The initial impedance R1 of the secondary battery was calculated as R1 = (V3 - V1) / 4C (unit: Ω). The secondary battery was left in a 60°C oven for one month, then taken out and returned to room temperature, and the secondary battery impedance R after storage was measured according to the test method for R1. 2 was measured, and the increase rate of the storage impedance was calculated as ΔR=R2 / R1×100%.
[0090] 3. Test capacity efficiency of the rate discharge after storage In test 2, the secondary battery after storage was charged to 4.35V at a constant current of 1C, and then charged at a constant voltage until the current was less than 0.05C. The secondary battery was then discharged to 2.8V at a constant current of 1C to obtain a 1C discharge capacity Q1. The secondary battery was charged to 4.35V at a constant current of 1C, and then charged at a constant voltage until the current was less than 0.05C. The secondary battery was then discharged to 2.8V at a constant current of 3C to obtain a 3C discharge capacity Q3. The rate discharge capacity efficiency was calculated as Q3 / Q1×100%.
[0091] 4. Cycling performance test at 45℃ At 45°C, the secondary battery was charged to 4.35 V at a constant current of 1 C, then charged at a constant voltage of 4.35 V until the current became less than 0.05 C, and then discharged to 2.8 V at a constant current of 1 C, which is one charge / discharge cycle. Charging and discharging were repeated in this manner, and the capacity retention rate of the secondary battery after 1000 cycles was calculated.
[0092] Capacity retention rate (%) of secondary battery after 1000 cycles at 45°C = (discharge capacity after 1000 cycles / discharge capacity of first cycle) x 100%.
[0093] [Table 1] TIFF0007569482000014.tif244170
[0094] [Table 2]
[0095] From an analysis of the parameters in Table 1 and the results in Table 2, the following was found: As is clear from the comparison of Comparative Examples 1, 2 and 6, when only the content of Co element is reduced to reduce the cost of the positive electrode material and the positive electrode material does not contain Al element, the self-discharge rate and the increase rate of storage impedance of the secondary battery are greatly increased, and even if vinylene carbonate (VC) is added to the electrolyte as an additive to suppress the reduction of the electrolyte solvent, the performance of the secondary battery cannot be effectively improved. In addition, as is clear from the comparison of Comparative Examples 2 and 3, by adding Al element to the positive electrode material with a reduced content of Co element, the self-discharge rate and the increase rate of storage impedance can be reduced to a certain extent, and the capacity efficiency of the rate discharge after storage can be improved. This is because the addition of Al element can reduce Li / Ni mixing due to the reduction of Co content and improve the structural stability of the positive electrode material, thereby improving the performance of the secondary battery to a certain extent. However, since the bond unsaturated structure of the surface of the positive electrode material becomes unstable, the Al element on the surface is easily involved in the reaction during charging and discharging, and therefore the role of completely stabilizing the surface of the material cannot be realized.
[0096] As is clear from the comparison between Example 1, Example 4 and Comparative Example 1 (see Table 3), by reducing the amount of Co element and using an appropriate amount of Al element, and by adding the compound represented by general formula (I) to the electrolyte, not only can the cost of the secondary battery be reduced by reducing the content of expensive Co, but also the self-discharge rate of the secondary battery can be reduced, the increase rate of the storage impedance can be reduced, and the capacity efficiency of the rate discharge after storage can be improved. This is because, by adding the compound represented by the above general formula (I) as an additive to the electrolyte, the compound is bonded with Al on the positive electrode surface in a certain direction during the first charge to form a chelate structure, and the two rings of the compound are opened and connected to each other to form a three-dimensional mesh structure, which is covered on the surface of the positive electrode particles, effectively stabilizing the Al element on the surface of the positive electrode material, and isolating the electrolyte and the positive electrode interface, thereby improving the stability and ion conductivity of the positive electrode surface structure, reducing side reactions at the interface, greatly reducing the self-discharge rate of the cell, reducing the increase rate of the storage impedance, improving the cycle stability of the battery, and improving the capacity efficiency of the rate discharge.
[0097] Also, as is clear from the comparison of Examples 2 to 6 and Comparative Examples 4 and 5, if the amount of Al element contained in the positive electrode is too small, it is insufficient to compensate for the decrease in performance of the secondary battery due to the decrease in the Co content. As the amount of Al element added gradually increases, sufficient Al element effectively reduces the Li / Ni mixing caused by the decrease in the Co content, stabilizes the stability of the bulk phase and surface structure of the positive electrode material, and combines the stabilizing effect of the compound additive represented by general formula (I) contained in the electrolyte on the Al element and the protective effect of the crosslinked network to greatly improve the performance of each secondary battery, which is superior to the performance of the secondary battery with a high Co content positive electrode system. As the amount of Al added increases continuously and exceeds a certain range, many inactive sites are formed in the positive electrode material, which limits the internal conduction and diffusion of lithium ions, and conversely reduces the ionic conductivity of the positive electrode material, thereby reducing the overall performance of the secondary battery. When the amount of Al added was in the preferred range of 1000-7000, the self-discharge rate of the secondary battery was <150mV / h, the increase rate of the storage impedance was <70%, and the capacity efficiency of the rate discharge was >93%, and the integrated performance was very good.
[0098] A comparison of Examples 4, 7-11 shows the effect of adjusting the specific surface area of the positive electrode material on the performance of the secondary battery. As the specific surface area of the positive electrode material gradually increases, the self-discharge rate also tends to increase, which is because the specific surface area directly affects the degree of side reactions at the interface. The larger the specific surface area, the more side reactions there are, and the higher the self-discharge rate. The increase in impedance after storage and the capacity efficiency of rate discharge tend to improve and then deteriorate, which is because a certain degree of side reaction plays a role in separating the interface of the positive electrode and the electrolyte, suppressing further occurrence of side reactions, thereby reducing the increase in impedance and improving the rate performance, but if the specific surface area is too large, the overall performance will be greatly deteriorated due to many side reactions. When the specific surface area of the positive electrode material is in the preferred range of 0.5-2.5, the self-discharge rate of the secondary battery is <100mV / h, the increase rate of storage impedance is <65%, and the capacity efficiency of rate discharge is >92%.
[0099] Examples 4, 12 to 24 show the effect of adding the compound represented by general formula (I) in different amounts or with different types or with other additives on the performance of the secondary battery. The results of the examples show that as the amount of the compound represented by general formula (I) added gradually increases, the self-discharge rate of the secondary battery gradually decreases, because a sufficient amount of the compound represented by general formula (I) reacts with the Al element to form a dense network structure on the surface of the positive electrode, thereby completely separating the positive electrode interface from the electrolyte, thereby reducing side reactions and reducing the self-discharge rate accordingly. On the other hand, the impedance increase after storage and the rate discharge capacity efficiency tend to improve and then deteriorate. This is because the amount of the compound of general formula (I) that can participate in stabilizing the Al element on the positive electrode surface gradually increases as the compound of general formula (I) gradually increases within a certain range. Combined with the protective effect of the network due to the ring-opening crosslinking of the compound of general formula (I) itself, the phase transition and side reaction at the interface are gradually reduced, and the impedance increase after storage and the rate discharge performance are effectively improved. However, if the compound of general formula (I) is added in an excessive amount, not only will it affect the stabilizing effect of chelation with Al, but also the impedance will increase significantly due to the unnecessary interface protection, the lithium ion transport path will be longer, and the difficulty of lithium ion transport will be improved, thus causing the impedance increase and the rate discharge capacity to deteriorate. When the compound of general formula (I) is added in a preferred range of 0.1-10%, the self-discharge rate of the secondary battery is <120mV / h, the storage impedance increase rate is <75%, and the rate discharge capacity efficiency is >92%, and the overall performance is greatly improved.
[0100] In addition, the compounds represented by general formula (I) all have the same performance improving effect. Furthermore, by using the compound represented by general formula (I) together with lithium difluoro(oxalato)borate (LiODFB) or fluoroethylene carbonate (FEC), a three-dimensional ion channel can be formed on the surface of the positive electrode, respectively, and side reactions at the interface of the negative electrode can be reduced, resulting in a better performance improving effect.
[0101] [Table 3]
[0102] [Table 4]
[0103] In addition, as can be seen from Table 4, in Examples 4, 14, 19, and 20, adding an appropriate amount of the compound of general formula (I) can improve the high-temperature cycle capacity retention rate of the secondary battery, which is mainly because the reduction of the side reaction on the positive electrode surface is favorable for improving the long-term stability of the positive electrode material interface, thereby further improving the cycle performance. Based on this, further adding LiODFB and FEC can further improve the ionic conductivity of the positive electrode material and improve the stability at the negative electrode interface, thereby further improving the high-temperature cycle performance of the secondary battery.
[0104] It should be noted that the present application is not limited to the above-mentioned embodiment. The above-mentioned embodiment is merely an example, and any embodiment having substantially the same configuration as the technical idea and exhibiting the same effect within the scope of the technical proposal of the present application is included in the technical scope of the present application. In addition, various modifications that a person skilled in the art can make to the embodiment without departing from the gist of the present application, and other forms combining some of the components in the embodiment are also included in the scope of the present application. [Explanation of symbols]
[0105] 1: Battery pack, 2: Upper housing, 3: Lower housing, 4: Battery module, 5: Secondary battery, 51: Housing, 52: Electrode assembly, 53: Top cover unit
Claims
1. The battery includes a positive electrode plate, a negative electrode plate, and an electrolyte solution, The positive electrode plate includes a positive electrode active material, the positive electrode active material including Ni, Co, Al, and Mn elements; In the positive electrode active material, the molar content of Co element satisfies Co≦0.09, and the mass content of Al element satisfies 500 ppm≦Al≦10000 ppm; The electrolyte solution contains a compound represented by the following general formula (I): [Formula 1] In the general formula (I), A 1 ~A 4 are each independently a single bond or an alkylene group having 1 to 5 carbon atoms; R 1 , R 1 ' are each independently [chemical 2] and R 2 teeth, [C3] and R 3 is an alkylene group or an alkyleneoxy group having 1 to 3 carbon atoms.
2. 2. The secondary battery according to claim 1, wherein the concentration of the compound of general formula (I) in the electrolyte is 0.01% by mass to 15% by mass.
3. In the general formula (I), A 1 ~A 4 and each independently represent a single bond or an alkylene group having 1 to 3 carbon atoms.
4. In the general formula (I), R 2 teeth, [C4] and R 3 The secondary battery according to any one of claims 1 to 3, wherein is an alkylene group or an alkyleneoxy group having 1 or 2 carbon atoms.
5. The secondary battery according to any one of claims 1 to 4, wherein the compound of general formula (I) is at least one selected from the following compounds 1 to 18. [C5]
6. The secondary battery according to any one of claims 1 to 5, wherein the mass content of the Al element satisfies 1000 ppm≦Al≦10000 ppm.
7. The general formula of the positive electrode active material is LiNi z Mn y Co x A a O 2 and x≦0.0 9, 0.0005≦a≦0.01, 0.5<z<1, 0<y<0.4, and x+y+z+a=1. The secondary battery according to any one of claims 1 to 6.
8. The secondary battery according to any one of claims 1 to 7, wherein the electrolyte further contains at least one other additive selected from lithium tetrafluoroborate, lithium bis(oxalato)borate, lithium difluoro(oxalato)borate, and tris(trimethylsilyl)borate.
9. The secondary battery according to claim 8, wherein the total concentration of the other additives in the electrolyte is 0.2% by mass to 3% by mass.
10. The specific surface area of the positive electrode active material is 0.5 to 3 m 2 The secondary battery according to any one of claims 1 to 9, wherein the molecular weight is 1 / g.
11. A power consuming device comprising the secondary battery according to any one of claims 1 to 10.
Citation Information
Patent Citations
A method for preparing doped and coated single-crystal ternary cathode material
CN109273710B
Ternary high-voltage lithium ion battery electrolyte and ternary high-voltage lithium ion battery
CN110021785A
Non-aqueous electrolyte and application thereof
CN111293357A
Electrolyte, preparation method thereof and lithium ion battery
CN112349958A
Organic electrolyte solution of 3,3,9,9-tetraoxide-2,4,8,10-tetraoxa-3,9-dithiaspiro[5.5]undecane for use in a lithium battery
EP3205655A1