Resin composition, molded article and multi-layer pipe

The resin composition for multilayer pipes, incorporating EVOH with a potassium salt and antioxidants, addresses delamination and interlayer adhesion issues, enhancing thermal stability and adhesion strength, making it suitable for hot water circulation systems.

JP7569629B2Active Publication Date: 2024-10-18KURARAY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020088262
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-20
Publication Date
2024-10-18
Estimated Expiration
2040-05-20

AI Technical Summary

Technical Problem

Multilayer pipes using ethylene-vinyl alcohol copolymer (EVOH) face issues with delamination, particularly when rapidly cooled during the manufacturing process, and also suffer from decreased interlayer adhesion strength, which can lead to corrosion of metal components in hot water circulation systems.

Method used

A resin composition containing EVOH, a potassium salt with a pKa of 4 to 6, a hindered phenolic antioxidant, and a conjugated polyene compound, optimized to maintain interlayer adhesion strength and thermal stability, with specific ethylene content and saponification degree, and controlled pH of the hot water extract.

Benefits of technology

The resin composition effectively suppresses delamination and maintains excellent hue and thermal stability, ensuring high interlayer adhesion strength even under rapid cooling conditions, suitable for use in hot water circulation pipes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569629000001
    Figure 0007569629000001
Patent Text Reader

Abstract

To provide a resin composition that can prevent delamination of a multilayer pipe produced in a process using EVOH even when quenched after melting and extrusion of the EVOH resin composition, and also has excellent hue and heat stability.SOLUTION: A resin composition contains an ethylene-vinyl alcohol copolymer (A), a potassium salt (B) and an antioxidant (C). The ethylene-vinyl alcohol copolymer (A) has an ethylene content of 15-60 mol% and a degree of saponification of 85 mol% or more. The potassium salt (B) is a potassium salt of a carboxylic acid with pKa of 4-6. The content of potassium salt (B) in terms of potassium is 200-1000 ppm relative to the ethylene-vinyl alcohol copolymer (A). The antioxidant (C) is a hindered phenolic antioxidant having an ester bond or amide bond. The content of the antioxidant (C) is 0.1-4 pts.mass relative to the ethylene-vinyl alcohol copolymer (A) 100 pts.mass.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a molded article, and a multi-layer pipe. [Background technology]

[0002] Traditionally, metal pipes have been mainly used for floor heating with hot water circulation. Hot water circulation pipes are often buried in concrete and installed under the floor during construction, making repairs difficult once installed, and they are usually required to last for a long period of about 50 years. Under such severe conditions, plastic pipes are preferably used, which are cheaper than metal pipes and do not involve the risk of pipe corrosion. Polyethylene, polypropylene, polybutene, etc. are used as plastic pipe materials.

[0003] On the other hand, when such plastic pipes are used for floor heating, there is a problem that metal parts such as heat exchangers and pumps are corroded by oxygen. The cause of this corrosion is thought to be oxygen in the air penetrating and dissolving in the hot water through the plastic pipe wall. Therefore, multi-layer polyethylene pipes with an aluminum intermediate layer were used, but the aluminum layer cracks, which are thought to be caused by temperature changes, and the problem of corrosion caused by oxygen penetration was not solved.

[0004] As a solution to this problem, various multi-layer pipes made of gas barrier resins and polyethylene have been used. Among them, multi-layer pipes using ethylene-vinyl alcohol copolymers (hereinafter sometimes abbreviated as EVOH) have excellent oxygen barrier properties and mechanical strength, and are now widely used as hot water circulation pipes. For example, hot water circulation pipes that include an EVOH layer as an intermediate layer (Patent Document 1) and hot water circulation pipes that have an EVOH layer as the outermost layer (Patent Document 2) are known. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 63-286459 [Patent Document 2] Japanese Patent Application Publication No. 4-227744 Summary of the Invention [Problem to be solved by the invention]

[0006] However, in multi-layer pipes using EVOH, delamination has sometimes been a problem. As a result of the investigation, it was found that when a multi-layer pipe using EVOH is subjected to rapid cooling after melt extrusion in the manufacturing process, the interlayer adhesive strength is reduced, and delamination of the resulting multi-layer pipe is likely to occur. In particular, in the case of a multi-layer pipe having an EVOH layer as the outermost layer, it was found that there is a high concern of delamination of the resulting multi-layer pipe due to the reduction in interlayer adhesive strength caused by particularly strong rapid cooling.

[0007] The present invention has been made based on the above-mentioned circumstances, and a first object of the present invention is to provide an EVOH resin composition which suppresses delamination in the resulting multi-layer pipe even when the EVOH resin composition is melt-extruded and then rapidly cooled in a process for producing a multi-layer pipe using EVOH. A second object of the present invention is to provide a resin composition which is excellent in hue and thermal stability and which can achieve both excellent hue and thermal stability of the resin composition and a high level of inhibition of delamination in the resulting multilayer pipe. [Means for solving the problem]

[0008] The present inventors have extensively studied the correlation between the resin composition of EVOH and the interlayer adhesive strength under various conditions, and have found that while sodium salts, which have been widely used to improve interlayer adhesive strength, cause a large decrease in interlayer adhesive strength under quenching conditions, the use of potassium salts can suppress the decrease in interlayer adhesive strength under quenching conditions. They have also found that the use of potassium salts can achieve a high level of both hue and interlayer adhesive strength of the resin composition. Although sodium and potassium belong to the same alkali metal group, it was a great surprise to find that they have such differences in properties. They have found that the above properties can be further improved by specifying the anion species constituting the potassium salt and the pH of the hot water extract of the resin composition, and have completed the invention. That is, the above problem is solved by: [1] A resin composition containing an ethylene-vinyl alcohol copolymer (A), a potassium salt (B), and an antioxidant (C), in which the ethylene-vinyl alcohol copolymer (A) has an ethylene content of 15 to 60 mol % and a degree of saponification of 85 mol % or more, the potassium salt (B) is a potassium salt of a carboxylic acid having a pKa of 4 to 6, the content of the potassium salt (B) relative to the ethylene-vinyl alcohol copolymer (A) is 200 to 1000 ppm in terms of potassium, the antioxidant (C) is a hindered phenol-based antioxidant having an ester bond or an amide bond, and the content of the antioxidant (C) relative to 100 parts by mass of the ethylene-vinyl alcohol copolymer (A) is 0.1 to 4 parts by mass; [2] The resin composition according to [1], wherein the potassium salt (B) is potassium acetate; [3] The resin composition of [1] or [2], in which a multilayer film having a layer made of the resin composition has an interlayer adhesive strength of 450 g / 15 mm or more as measured under the evaluation conditions described in the Examples; [4] A resin composition containing an ethylene-vinyl alcohol copolymer (A), wherein a multilayer film having a layer made of the resin composition has an interlayer adhesive strength of 450 g / 15 mm or more as measured under the evaluation conditions described in the examples; [5] The resin composition according to any one of [1] to [4], further comprising a conjugated polyene compound (D), wherein the content of the conjugated polyene compound (D) per 100 parts by mass of the ethylene-vinyl alcohol copolymer (A) is 0.001 to 0.15 parts by mass; [6] The resin composition according to any one of [1] to [5], wherein 10 g of the resin composition is placed in 50 ml of pure water and extracted at 95°C for 8 hours, and the pH of the extract at 20°C is 4.0 to 5.5; [7] A molded article having at least one layer made of the resin composition according to any one of [1] to [6]; [8] A multilayer pipe having at least one layer made of the resin composition according to any one of [1] to [6]; [9] A multilayer pipe having a layer made of any one of the resin compositions according to [1] to [6] as an outermost layer;

[10] A method for producing a multi-layer pipe having at least one layer made of the resin composition according to any one of [1] to [6], comprising a step of cooling each layer constituting the multi-layer pipe with water or air at 10 to 50°C immediately after extrusion from a die; This is solved by providing Effect of the Invention

[0009] The resin composition of the present invention can suppress delamination of the resulting multi-layer pipe even when the EVOH resin composition is melt-extruded and then rapidly cooled in the manufacturing process of the multi-layer pipe using EVOH. Furthermore, the resin composition of the present invention is excellent in color and thermal stability, and can achieve both excellent color and thermal stability of the resin composition and suppression of delamination of the resulting multi-layer pipe at a high level. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present invention will be described. In the following description, specific materials (compounds, etc.) that exhibit specific functions may be exemplified, but the present invention is not limited to the embodiment using such materials. Furthermore, the exemplified materials may be used alone or in combination, unless otherwise specified.

[0011] <EVOH(A)> EVOH (A) is the main component of the resin composition of the present invention. EVOH (A) is a copolymer having ethylene units and vinyl alcohol units as main structural units. EVOH (A) is usually obtained by polymerizing ethylene and vinyl ester and saponifying the resulting ethylene-vinyl ester copolymer. The main component indicates that the content of EVOH (A) in the resin constituting the resin composition of the present invention is 70 mass% or more, preferably 80 mass% or more, more preferably 90 mass% or more, particularly preferably 95 mass% or more, and may be 99 mass% or more. By setting the content of EVOH (A) within this range, the gas barrier property of the resulting resin composition is excellent.

[0012] The gas barrier properties of the resin composition can be measured by a known method. For example, a single-layer film having a thickness of 20 μm is obtained using the resin composition, and the oxygen transmission rate [unit: cc 20 μm / (m )] is measured using an oxygen transmission rate measuring device (MOCON OX-TRAN2 / 20 manufactured by Modern Controls) under the following conditions: temperature 20° C., humidity of the oxygen supply side and carrier gas side 85% RH, oxygen pressure of 1 atm, and carrier gas pressure of 1 atm. 2 1. ·day·atm) can be used as the carrier gas. Nitrogen gas containing 2% by volume of hydrogen gas can be used as the carrier gas. The following conditions may be used as the extrusion conditions for the monolayer film. The thickness of the monolayer film can be adjusted by changing the take-up roll speed. Extruder: Toyo Seiki single screw extruder Screw diameter: 20mmφ (L / D=20, compression ratio=3.5, full flight type) Screw rotation speed: 40 rpm Extrusion temperature: C1 / C2 / C3 / die = 190 / 220 / 220 / 220℃ Take-up roll temperature: 80℃

[0013] The ethylene unit content of EVOH (A), i.e., the ratio of the number of ethylene units to the total number of monomer units in EVOH (A), is in the range of 15 to 60 mol%. The lower limit of the ethylene unit content of EVOH (A) is preferably 20 mol%, more preferably 23 mol%. On the other hand, the upper limit of the ethylene unit content of EVOH (A) is preferably 55 mol%, more preferably 50 mol%. If the ethylene unit content of EVOH (A) is less than 15 mol%, the gas barrier property under high humidity may decrease, and the melt moldability may also deteriorate. If the ethylene unit content of EVOH (A) exceeds 60 mol%, sufficient gas barrier property may not be obtained.

[0014] The degree of saponification of EVOH (A), i.e., the ratio of the number of vinyl alcohol units to the total number of vinyl alcohol units and vinyl ester units in EVOH (A), is 85 mol% or more. The lower limit of the degree of saponification of EVOH (A) is preferably 95 mol%, more preferably 99 mol%. On the other hand, the upper limit of the degree of saponification of EVOH (A) is preferably 100 mol%, more preferably 99.99 mol%. If the degree of saponification of EVOH (A) is less than 85 mol%, sufficient gas barrier properties may not be obtained, and further, thermal stability may be insufficient.

[0015] EVOH (A) may be a mixture of two or more kinds of EVOH having different ethylene unit contents. In this case, the difference in ethylene unit contents between the EVOH having the most different ethylene unit contents is preferably 30 mol% or less, more preferably 20 mol% or less, and even more preferably 15 mol% or less. Similarly, EVOH (A) may be a mixture of two or more kinds of EVOH having different saponification degrees. In this case, the difference in saponification degrees between the EVOH having the most different ethylene unit contents is preferably 7% or less, more preferably 5% or less. When a resin composition having both thermoformability and gas barrier properties at a higher level is desired, it is preferable to mix EVOH (A-1) having an ethylene unit content of 24 mol% or more and less than 34 mol% and a saponification degree of 99 mol% or more with EVOH (A-2) having an ethylene unit content of 34 mol% or more and less than 50 mol% and a saponification degree of 99 mol% or more in a blending mass ratio (A-1 / A-2) of 60 / 40 to 90 / 10 and use the mixture as EVOH (A). The ethylene unit content and the degree of saponification of EVOH (A) can be determined by a nuclear magnetic resonance (NMR) method.

[0016] The lower limit of the melt flow rate (hereinafter sometimes simply abbreviated as "MFR") of EVOH (A) according to JIS K 7210:2014 (temperature 210°C, load 2160g) is preferably 0.1g / 10min, more preferably 0.5g / 10min, and even more preferably 1g / 10min. On the other hand, the upper limit of the MFR of EVOH (A) is preferably 50g / 10min, more preferably 30g / 10min, and even more preferably 15g / 10min. By setting the MFR of EVOH (A) to a value within this range, the melt moldability of the obtained resin composition is improved.

[0017] EVOH (A) may contain monomer units other than ethylene units, vinyl alcohol units and vinyl ester units as copolymerization units within the scope of the present invention. Examples of the monomers include α-olefins such as propylene, 1-butene, isobutene, 4-methyl-1-pentene, 1-hexene, and 1-octene; unsaturated carboxylic acids such as itaconic acid, methacrylic acid, acrylic acid, and maleic acid, their salts, partial or complete esters, their nitriles, their amides, and their anhydrides; vinylsilane-based compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, vinyltri(β-methoxyethoxy)silane, and γ-methacryloxypropyltrimethoxysilane; unsaturated sulfonic acids or their salts; unsaturated thiols; and vinylpyrrolidones. The content of monomer units other than ethylene units, vinyl alcohol units, and vinyl ester units in EVOH (A) is usually 5 mol% or less, preferably 2 mol% or less, and more preferably 1 mol% or less.

[0018] EVOH is usually synthesized by saponifying an ethylene-vinyl ester copolymer, and vinyl acetate is generally used as the vinyl ester. When ethylene and vinyl acetate are copolymerized, other fatty acid vinyl esters (vinyl propionate, vinyl pivalate, etc.) can also be used in combination.

[0019] The polymerization of ethylene and vinyl ester may be any of solution polymerization, suspension polymerization, emulsion polymerization, and bulk polymerization, and may be any of continuous and batch systems. For example, the polymerization conditions for batch system solution polymerization are as follows:

[0020] Solvent: Alcohols are preferred, but other organic solvents capable of dissolving ethylene, vinyl ester, and ethylene-vinyl ester copolymers (e.g., dimethyl sulfoxide) can be used. Examples of alcohols that can be used include methyl alcohol, ethyl alcohol, propyl alcohol, n-butyl alcohol, and t-butyl alcohol, with methyl alcohol being particularly preferred. Catalyst: Azonitrile-based initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis-(2,4-dimethylvaleronitrile), 2,2'-azobis-(4-methyl-2,4-dimethylvaleronitrile), 2,2'-azobis-(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis-(2-cyclopropylpropionitrile), and organic peroxide-based initiators such as isobutyryl peroxide, cumyl peroxy neodecanoate, diisopropyl peroxy dicarbonate, di-n-propyl peroxy dicarbonate, t-butyl peroxy neodecanoate, lauroyl peroxide, benzoyl peroxide, t-butyl hydroperoxide, and the like can be used. Temperature: 20 to 90°C, preferably 40 to 70°C. Time: 2 to 15 hours, preferably 3 to 11 hours. Polymerization rate: 10 to 90%, preferably 30 to 80%, based on the charged vinyl ester. Resin content in the solution after polymerization: 5 to 85%, preferably 20 to 70%.

[0021] In addition to ethylene and vinyl ester, it is also possible to allow a small amount of a monomer that can be copolymerized with them to coexist. Examples of the copolymerizable monomer include α-olefins such as propylene, isobutylene, α-octene, and α-dodecene; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, and itaconic acid, or their anhydrides, salts, or mono- or dialkyl esters; vinyl silanes such as vinyl trimethoxy silane, vinyl triethoxy silane, vinyl tri(β-methoxy-ethoxy) silane, and γ-methacryloxypropyl methoxy silane; nitriles such as acrylonitrile and methacrylonitrile; amides such as acrylamide and methacrylamide; olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid, or their salts; alkyl vinyl ethers, vinyl ketones, N-vinyl pyrrolidone, vinyl chloride, and vinylidene chloride.

[0022] After a predetermined time of polymerization, when a predetermined polymerization rate is reached, a polymerization inhibitor is added as necessary, unreacted ethylene gas is removed by evaporation, and unreacted vinyl acetate is removed. As a method for removing unreacted vinyl acetate from the ethylene-vinyl acetate copolymer from which ethylene has been removed by evaporation, for example, a method is adopted in which the copolymer solution is continuously fed at a constant rate from the top of a tower packed with Raschig rings, an organic solvent vapor such as methanol is blown into the bottom of the tower, a mixed vapor of the organic solvent such as methanol and unreacted vinyl acetate is distilled from the top of the tower, and the copolymer solution from which unreacted vinyl acetate has been removed is taken out from the bottom of the tower.

[0023] An alkali catalyst is added to the copolymer solution from which unreacted vinyl acetate has been removed, and the vinyl acetate component in the copolymer is saponified. The saponification method can be either continuous or batchwise. As the alkali catalyst, sodium hydroxide, potassium hydroxide, alkali metal alcoholate, etc. are used. For example, the saponification conditions in the batchwise method are as follows: The copolymer solution concentration: 10-50%. Reaction temperature: 30~60℃. Amount of catalyst used: 0.02 to 0.6 equivalents (per vinyl acetate component). Time: 1-6 hours. It is also common to add an acid such as acetic acid after the saponification step to neutralize any remaining alkaline catalyst.

[0024] Examples of the granulation procedure include (1) a method in which a solution containing EVOH is extruded into a low-temperature poor solvent to precipitate or solidify, and then cut immediately thereafter or after further cooling and solidification, and (2) a method in which a solution of EVOH is contacted with water vapor to obtain a hydrous EVOH resin composition in advance, and then the hydrous resin composition is cut. The water content in the hydrous EVOH pellets obtained by these methods is preferably 50 to 200 parts by mass, more preferably 70 to 150 parts by mass, based on 100 parts by mass of EVOH.

[0025] <Potassium salt (B)> In a first embodiment of the present invention, the resin composition contains a potassium salt (B) of a carboxylic acid having a pKa of 4 to 6. By containing the potassium salt (B) in the resin composition of the present invention, sufficient interlayer adhesion can be exhibited even when the resin composition is quenched after melt extrusion in the manufacturing process of the multilayer pipe, and the hue of the resin composition and the suppression of interlayer peeling of the obtained multilayer pipe can be compatible.

[0026] The reason is that potassium ions have a higher mobility in EVOH than sodium ions, and are believed to be able to promote the interlayer adhesion reaction more efficiently, resulting in significantly better interlayer adhesion, especially when quenched. In addition, by controlling the content ratio with the carboxylic acid described below, the color and melt moldability of the resulting resin composition can be further improved.

[0027] The content of the potassium salt (B) is 200 to 1000 ppm in terms of potassium relative to the ethylene-vinyl alcohol copolymer (A). If the content is less than 200 ppm, the interlayer adhesive strength may be insufficient, and the resulting multilayer pipe may not be sufficiently prevented from peeling. On the other hand, if the content is more than 1000 ppm, the color may deteriorate. The lower limit of the content is preferably 250 ppm. On the other hand, the upper limit of the content is preferably 500 ppm.

[0028] The pKa of the carboxylic acid of the potassium salt (B) must be in the range of 4 to 6. When the pKa of the carboxylic acid of the potassium salt (B) is in the above range, the interlayer adhesive strength becomes sufficient, and the pH buffering ability of the resulting resin composition is increased, and the coloring resistance to acidic and basic substances may be improved. In the case of polyacids, it is sufficient that the pKa of at least one acid is in the range of 4 to 6. Carboxylic acids of the potassium salt (B) that satisfy such conditions include acetic acid (pKa = 4.76), propionic acid (pKa = 4.85), acrylic acid (pKa = 4.25), oxalic acid (pKa2 = 4.27), succinic acid (pKa1 = 4.20), fumaric acid (pKa2 = 4.44), malic acid (pKa2 = 5.13), glutaric acid (pKa1 = 4.30, pKa2 = 5.4). 0), adipic acid (pKa1=4.43, pKa2=5.41), pimelic acid (pKa1=4.71), phthalic acid (pKa2=5.41), isophthalic acid (pKa2=4.46), terephthalic acid (pKa1=3.51, pKa2=4.82), citric acid (pKa2=4.75), tartaric acid (pKa2=4.40), glutamic acid (pKa2=4.07), etc. Among these, potassium acetate or citric acid is preferred from the standpoint of safety, handling, and economy, and potassium acetate is more preferred.

[0029] <Antioxidants (C)> In a first embodiment of the present invention, the resin composition contains a hindered phenol-based antioxidant (C) having an ester bond or an amide bond. By containing the antioxidant (C) in the resin composition of the present invention, the thermal stability is improved and stable physical properties can be maintained for a long period of time. In particular, when a multi-layer pipe described later is laid in concrete or underground as a hot water circulation pipe and used for a long period of time, oxidation deterioration of the resin composition constituting the multi-layer pipe can be effectively suppressed.

[0030] The content of the antioxidant (C) is 0.1 to 4 parts by mass relative to 100 parts by mass of the ethylene-vinyl alcohol copolymer (A). If the content is less than 0.1 parts by mass, the thermal stability may be insufficient. If the content is more than 4 parts by mass, the hue and melt moldability of the resulting resin composition may decrease, or bleeding out of the antioxidant (C) may become a problem. The lower limit of the content is preferably 0.3 parts by mass. On the other hand, the upper limit of the content is preferably 2 parts by mass.

[0031] The antioxidant (C) has at least one hindered phenol group. The hindered phenol group refers to a bulky substituent bonded to at least one of the carbons adjacent to the carbon to which the hydroxyl group of phenol is bonded. As the bulky substituent, an alkyl group having 1 to 10 carbon atoms is preferable, and a t-butyl group is more preferable. The antioxidant (C) needs to have an ester bond or an amide bond. The antioxidant (C) having an ester bond may be an ester of an aliphatic carboxylic acid having a hindered phenol group and an aliphatic alcohol, and the antioxidant (C) having an amide bond may be an amide of an aliphatic carboxylic acid having a hindered phenol group and an aliphatic amine. Among them, it is preferable that the antioxidant (C) has an amide bond from the viewpoint of good dispersibility in EVOH (A) and efficient expression of antioxidant performance.

[0032] The antioxidant (C) is preferably in a solid state at about room temperature. From the viewpoint of suppressing bleed-out of the antioxidant (C), the melting point or softening temperature of the antioxidant (C) is preferably 50° C. or higher, more preferably 60° C. or higher, and even more preferably 70° C. or higher. From the viewpoint of facilitating mixing with the EVOH (A), the melting point or softening temperature of the antioxidant (C) is preferably 200° C. or lower, more preferably 190° C. or lower, and even more preferably 180° C. or lower. From the viewpoint of suppressing bleed-out of the antioxidant (C), the molecular weight of the antioxidant (C) is preferably at least 200, more preferably at least 400, and even more preferably at least 600. On the other hand, the molecular weight is usually at most 2000.

[0033] Specific structures of the antioxidant (C) include pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] commercially available from BASF as Irganox 1010, 3-(3,5-di-tert-butyl-4-hydroxyphenyl)stearylpropionate commercially available as Irganox 1076, 2,2'-thiodiethylbis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] commercially available as Irganox 1035, and 3-(3 octadecyl bis(3-tert-butyl-4-hydroxyphenyl)propanoate, ethylene bis(oxyethylene) bis(3-tert-butyl-4-hydroxy-5-methylbenzenepropanoate) available commercially as Irganox 245, 1,6-hexanediol bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] available commercially as Irganox 259, and N,N'-hexamethylene bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide] available commercially as Irganox 1098. Among these, N,N'-hexamethylenebis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propanamide], commercially available as Irganox 1098, and pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], commercially available as Irganox 1010, are preferred, with the former being more preferred.

[0034] <Conjugated polyene compound (D)> The resin composition of the present invention may further contain a conjugated polyene compound (D). By containing the conjugated polyene compound (D), the resin composition of the present invention has improved thermal stability and can maintain stable physical properties for a long period of time.

[0035] The content of the conjugated polyene compound (D) is preferably 0.001 to 0.15 parts by mass relative to 100 parts by mass of the ethylene-vinyl alcohol copolymer (A). If the content is less than 0.001 parts by mass, the thermal stability may be insufficient. If the content is more than 0.15 parts by mass, the hue and melt moldability of the resulting resin composition may be deteriorated. The lower limit of the content is more preferably 0.003 parts by mass. On the other hand, the upper limit of the content is more preferably 0.10 parts by mass.

[0036] The conjugated polyene compound (D) is a compound having a structure in which carbon-carbon double bonds and carbon-carbon single bonds are alternately connected, and the number of carbon-carbon double bonds is two or more, that is, a so-called conjugated double bond. It may be a conjugated diene having a structure in which two carbon-carbon double bonds and one carbon-carbon single bond are alternately connected, a conjugated triene having a structure in which three carbon-carbon double bonds and two carbon-carbon single bonds are alternately connected, or a conjugated polyene compound having a structure in which a greater number of carbon-carbon double bonds and carbon-carbon single bonds are alternately connected. However, since there is a possibility that the conjugated polyene compound itself may be colored when the number of conjugated carbon-carbon double bonds is eight or more, it is preferable that the polyene compound has seven or less conjugated carbon-carbon double bonds. In addition, the above-mentioned conjugated double bonds consisting of two or more carbon-carbon double bonds may be present in a single molecule in a plurality of pairs without being conjugated with each other. For example, a compound having three conjugated trienes in the same molecule, such as tung oil, is also included in the conjugated polyene compound (D) of the present invention. Furthermore, in addition to the conjugated double bond, other functional groups such as a carboxyl group and salts thereof, a hydroxyl group, an ester group, a carbonyl group, an ether group, an amino group, an imino group, an amide group, a cyano group, a diazo group, a nitro group, a sulfone group and salts thereof, a sulfonyl group, a sulfoxide group, a sulfide group, a thiol group, a phosphate group and salts thereof, a phenyl group, a halogen atom, a double bond, or a triple bond may be contained.

[0037] From the viewpoint of improving dispersibility in EVOH (A), the molecular weight of the conjugated polyene compound (D) is preferably 1000 or less, more preferably 500 or less, and even more preferably 300 or less.

[0038] Specific examples of the conjugated polyene compound (D) include isoprene, 2,3-dimethyl-1,3-butadiene, 2,3-diethyl-1,3-butadiene, 2-t-butyl-1,3-butadiene, 1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 2,4-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-pentadiene, 3-ethyl-1,3-pentadiene, and 2-methyl-1,3-pentadiene. , 3-methyl-1,3-pentadiene, 4-methyl-1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 2,5-dimethyl-2,4-hexadiene, 1,3-octadiene, 1,3-cyclopentadiene, 1,3-cyclohexadiene, 1-phenyl-1,3-butadiene, 1,4-diphenyl-1,3-butadiene, 1-methoxy-1,3-butadiene, 2-methoxy-1,3-butadiene, 1 -Ethoxy-1,3-butadiene, 2-ethoxy-1,3-butadiene, 2-nitro-1,3-butadiene, chloroprene, 1-chloro-1,3-butadiene, 1-bromo-1,3-butadiene, 2-bromo-1,3-butadiene, fulvene, tropone, ocimene, phellandrene, myrcene, farnesene, cembrene, sorbic acid, sorbic acid esters, sorbates, abietic acid, etc. Conjugated dienes having a conjugated structure; conjugated trienes having a conjugated structure with three carbon-carbon double bonds, such as 1,3,5-hexatriene, 2,4,6-octatriene-1-carboxylic acid, eleostearic acid, tung oil, and cholecalciferol; conjugated polyenes having a conjugated structure with four or more carbon-carbon double bonds, such as cyclooctatetraene, 2,4,6,8-decatetraene-1-carboxylic acid, retinol, and retinoic acid. Two or more of such polyene compounds can be used in combination. Among them, sorbic acid, sorbic acid esters, sorbic acid salts, myrcene such as β-myrcene, and mixtures thereof are preferred, and at least one selected from the group consisting of sorbic acid, sorbic acid esters, and sorbic acid salts is preferred from the viewpoints of hygiene and availability, and also effective in suppressing oxidation deterioration at high temperatures.

[0039] The resin composition of the present invention may contain other components other than EVOH (A), potassium salt (B), antioxidant (C) and conjugated polyene compound (D) as long as the effects of the present invention are not impaired. Examples of other components include alkali metal ions other than potassium, alkaline earth metal ions and transition metal ions, carboxylic acids, phosphoric acid compounds, boron compounds, oxidation promoters, antioxidants other than the antioxidant (C), plasticizers, heat stabilizers (melt stabilizers), photoinitiators, deodorants, ultraviolet absorbers, antistatic agents, lubricants, colorants, fillers, drying agents, bulking agents, pigments, dyes, processing aids, flame retardants, and antifogging agents. In particular, from the viewpoint of improving hue and melt moldability, it is preferable to contain carboxylic acids and phosphoric acid compounds. In addition, from the viewpoint of improving material recyclability, it is preferable to contain alkaline earth metal ions. Furthermore, from the viewpoint of improving melt viscosity and mechanical properties, it is preferable to contain a boron compound. The content of other components in the resin composition of the present invention is usually 5% by mass or less, preferably 3% by mass or less, and more preferably 1% by mass or less.

[0040] <Alkaline earth metal ions> The resin composition of the present invention may further contain alkaline earth metal ions. The lower limit of the alkaline earth metal ion content is preferably 10 ppm. Meanwhile, the upper limit of the alkaline earth metal ion content is preferably 200 ppm. By setting the alkaline earth metal ion content in this range, the resin composition of the present invention may suppress thickening and crosslinking behavior, thereby suppressing the occurrence of gels and bumps.

[0041] Examples of alkaline earth metal ions include magnesium, calcium, strontium, and barium ions, but magnesium or calcium ions are preferred from the viewpoints of small effect on coloration and ease of industrial availability. Magnesium ions are particularly preferred from the viewpoint of effectively suppressing the generation of gels and bumps with a small content, but calcium ions are preferred from the viewpoint of achieving compatibility with hue. These ions may be used alone or in combination of two or more.

[0042] Examples of alkaline earth metal salts that provide alkaline earth metal ions include aliphatic carboxylates, aromatic carboxylates, carbonates, hydrochlorides, nitrates, sulfates, phosphates, and metal complexes of magnesium, calcium, etc. Among these, magnesium acetate and calcium acetate are more preferred because they are easily available.

[0043] <Carboxylic acid> The resin composition of the present invention may further contain a carboxylic acid. The lower limit of the content of the carboxylic acid is preferably 50 ppm, more preferably 100 ppm. On the other hand, the upper limit of the content of the carboxylic acid is preferably 400 ppm, more preferably 350 ppm. When the content of the carboxylic acid is less than 50 ppm, the coloring resistance may be insufficient. On the other hand, when the content of the carboxylic acid is more than 400 ppm, the interlayer adhesive strength may be insufficient or odor may become a problem. The content of the carboxylic acid is determined by extracting 10 g of the resin composition with 50 ml of pure water at 95 ° C for 8 hours, and then titrating the resulting extract with an aqueous sodium hydroxide solution using phenolphthalein as an indicator. The content of the carboxylic acid does not take into account the carboxylic acid present as a salt in the extract. In addition, when the resin composition of the present invention contains acidic compounds other than the carboxylic acid, the content of the carboxylic acid in the resin composition can be determined by subtracting the contribution of these acidic compounds from the measured value by titration.

[0044] The pKa of the carboxylic acid is preferably 4 to 6. When the pKa of the carboxylic acid is within the above range, the pH buffering ability of the resulting resin composition is increased, and the melt moldability is further improved, and coloration due to acidic or basic substances can be further improved.

[0045] The carboxylic acid may be a monobasic carboxylic acid or a polybasic carboxylic acid, and these may be used alone or in combination of two or more kinds. A monocarboxylic acid is a compound having one carboxyl group in the molecule. Examples of monocarboxylic acids having a pKa in the range of 4 to 6 include acetic acid (pKa = 4.76), propionic acid (pKa = 4.85), and acrylic acid (pKa = 4.25). Among them, acetic acid is preferred because of its high safety, availability, and ease of handling. These carboxylic acids may further have a substituent such as a hydroxyl group, an amino group, or a halogen atom.

[0046] A polycarboxylic acid is a compound having two or more carboxyl groups in the molecule. In this case, it is preferable that the pKa of at least one carboxyl group is in the range of 4 to 6, and examples of such acids include oxalic acid (pKa2=4.27), succinic acid (pKa1=4.20), fumaric acid (pKa2=4.44), malic acid (pKa2=5.13), glutaric acid (pKa1=4.30, pKa2=5.40), adipic acid (pKa1=4.43, pKa2= 5.41), pimelic acid (pKa1 = 4.71), phthalic acid (pKa2 = 5.41), isophthalic acid (pKa2 = 4.46), terephthalic acid (pKa1 = 3.51, pKa2 = 4.82), citric acid (pKa2 = 4.75), tartaric acid (pKa2 = 4.40), glutamic acid (pKa2 = 4.07), aspartic acid (pKa = 3.90), etc.

[0047] When the carboxylic acid is a polycarboxylic acid, the coloring resistance at high temperatures may be further improved. It is also preferable that the polycarboxylic acid has three or more carboxyl groups. In this case, the coloring resistance may be more effectively improved.

[0048] <Phosphate compounds> The resin composition of the present invention may further contain a phosphoric acid compound. The lower limit of the content of the phosphoric acid compound is preferably 5 ppm in terms of phosphoric acid radicals. On the other hand, the upper limit of the content of the phosphoric acid compound is preferably 100 ppm in terms of phosphoric acid radicals. By containing the phosphoric acid compound in this range, color resistance and melt moldability may be improved.

[0049] As the phosphoric acid compound, for example, various acids such as phosphoric acid and phosphorous acid and their salts can be used. The phosphate may be any of primary phosphate, secondary phosphate, and tertiary phosphate. The cationic species of the phosphate is not particularly limited.

[0050] <Boron compounds> The resin composition of the present invention may further contain a boron compound. The lower limit of the content of the boron compound is preferably 15 ppm in terms of boron element. On the other hand, the upper limit of the content of the boron compound is preferably 300 ppm in terms of boron element. By containing the boron compound in this range, the melt viscosity may be improved and mechanical properties may be improved.

[0051] Examples of boron compounds include boric acid, boric acid esters, borate salts, and boron hydrides.Specific examples include boric acids such as orthoboric acid (H3BO3), metaboric acid, and tetraboric acid; boric acid esters such as trimethyl borate and triethyl borate; alkali metal salts or alkaline earth metal salts of the boric acid, and borate salts such as borax.Of these, orthoboric acid is preferred.

[0052] The resin composition of the present invention may further contain a thermoplastic resin other than EVOH (A). Examples of the thermoplastic resin other than EVOH (A) include various polyolefins (polyethylene, polypropylene, poly1-butene, poly4-methyl-1-pentene, ethylene-propylene copolymers, copolymers of ethylene and α-olefins having 4 or more carbon atoms, copolymers of polyolefins and maleic anhydride, ethylene-vinyl ester copolymers, ethylene-acrylic acid ester copolymers, or modified polyolefins obtained by graft-modifying these with unsaturated carboxylic acids or their derivatives, etc.), various polyamides (nylon 6, nylon 6·6, nylon 6 / 66 copolymers, nylon 11, nylon 12, polymetaxylylene adipamide, etc.), various polyesters (polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, etc.), polyvinyl chloride, polyvinylidene chloride, polystyrene, polyacrylonitrile, polyurethane, polycarbonate, polyacetal, polyacrylate, and modified polyvinyl alcohol resins, etc. The content of the thermoplastic resin in the resin composition of the present invention is less than 30% by mass, preferably less than 20% by mass, more preferably less than 10% by mass, even more preferably 5% by mass or less, and may be 1% by mass or less.

[0053] <Resin composition> In the first embodiment of the present invention, it is preferable that the pH of the extract obtained by adding 10 g of the resin composition to 50 ml of pure water and extracting at 95° C. for 8 hours is 4.0 to 5.5 at 20° C. When the pH is within the above range, it is possible to achieve a high level of both the hue and melt moldability of the resin composition, and the inhibition of delamination of the obtained multi-layer pipe. The pH can be controlled by the type and amount of the potassium salt (B), alkali metal ions other than potassium, alkaline earth metal ions, carboxylic acids, phosphoric acid compounds, etc.

[0054] In a second embodiment of the present invention, the resin composition has a YI (yellow index) of less than 24, and a multilayer film having a layer made of the resin composition has an interlayer adhesion strength of 450 g / 15 mm or more measured under the evaluation conditions described in the Examples below. This allows the obtained multilayer pipe to have excellent appearance and excellent suppression of interlayer peeling, and can be preferably used in particular for a multilayer pipe having an EVOH layer as the outermost layer.

[0055] <Method of producing resin composition> In the first embodiment, the method for producing the resin composition of the present invention is not limited as long as the EVOH (A), the potassium salt (B), and the antioxidant (C) are ultimately contained in the above-mentioned ranges. However, it is preferable to produce the resin composition by the production method of the present invention described below.

[0056] In the first embodiment of the present invention, the method of incorporating the potassium salt (B) into the resin composition is not particularly limited, but for example, a method of immersing a hydrous pellet containing EVOH (A) in a solution in which the potassium salt (B) is dissolved is preferred. In this case, the shape of the EVOH (A) may be any shape such as powder, granules, spheres, cylindrical pellets, etc. The concentration of the potassium salt (B) in the solution is not particularly limited. The solvent of the solution is also not particularly limited, but an aqueous solution is preferred from the viewpoints of ease of handling and environmental impact. The immersion time varies depending on the form of EVOH (A), but in the case of pellets of about 1 to 10 mm, it is preferably 1 hour or more, more preferably 2 hours or more. When the resin composition is immersed in the solution as described above, a resin composition with a volatile content of less than 0.3% can be obtained by drying at the end. On the other hand, the method of incorporating the antioxidant (C) into the resin composition of the present invention is also not particularly limited, but for example, a method of melting EVOH (A) and mixing the antioxidant (C) is preferred. The antioxidant (C) may be blended in a solid state such as powder, or as a melt, or may be blended as a solute contained in a solution or a dispersoid contained in a dispersion. As the solution and dispersion, an aqueous solution and an aqueous dispersion are preferable, respectively. For melt kneading, a known mixing or kneading device such as a kneader-ruder, an extruder, a mixing roll, or a Banbury mixer can be used. The temperature range during melt kneading can be appropriately adjusted depending on the melting point of the EVOH (A) used, and is usually 150 to 300°C. Other components such as a conjugated polyene compound (D), an alkaline earth metal ion, a carboxylic acid, a phosphoric acid compound, and a boron compound can also be incorporated by any of the above methods.

[0057] The resin composition of the present invention can be obtained, for example, by drying the hydrous pellets of EVOH obtained in the granulation step of EVOH (A) described above. The volatile content of the resin composition of the present invention is preferably less than 0.5% by mass, more preferably less than 0.3% by mass. Examples of the drying method for the hydrous pellets include static drying and fluidized drying. These drying methods may be used alone or in combination. The drying process may be performed by either a continuous method or a batch method. When a combination of a plurality of drying methods is used, the continuous method or the batch method can be freely selected for each drying method. From the viewpoint of reducing deterioration of the pellets due to oxygen during drying, it is also preferable to perform the drying in a low oxygen concentration or in an oxygen-free state. The drying temperature is usually less than 150°C.

[0058] <Molded body> The resin composition of the present invention can be processed into various molded articles by various melt molding methods. The molded article thus obtained is also one aspect of the present invention. The molded article of the present invention may be, for example, a molded article having a single layer structure or a multi-layer molded article having at least one layer made of the resin composition of the present invention. The molding method may be, for example, extrusion molding, thermoforming, profile molding, blow molding, rotational molding, or injection molding. Suitable applications of the molded article of the present invention include, for example, films, sheets, containers, bottles, tanks, pipes, hoses, and the like. In particular, a multi-layer pipe having at least one layer made of the resin composition of the present invention is a suitable embodiment of the present invention.

[0059] A preferred embodiment of the molded article obtained from the resin composition of the present invention is a multi-layer molded article having at least one layer made of the resin composition of the present invention. The multi-layer structure preferably further includes a layer obtained from a thermoplastic resin other than EVOH (A). The multi-layer structure also preferably includes a layer obtained from an adhesive resin. The layer structure of the multi-layer molded article is not particularly limited, but when the layer obtained from the resin composition of the present invention is represented by E, the layer obtained from the adhesive resin by Ad, and the layer obtained from the other thermoplastic resin by T, the following layer structure can be exemplified. Here, as the adhesive resin, a polyolefin modified with an unsaturated carboxylic acid or a derivative thereof is preferably used. In addition, as the thermoplastic resin, polyolefins such as polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, etc. can be mentioned, among which polyethylene is preferred, and high-density polyethylene is particularly preferred. In addition, in such a multi-layer molded article, the other thermoplastic resin and / or adhesive resin can be substituted with scraps of the multi-layer molded article. Scraps of other polyolefin molded articles can also be mixed and used. 2 layer Ad / E 3 layers T / Ad / E, Ad / E / Ad, E / Ad / E 4 layers T / Ad / E / Ad, Ad / E / Ad / E 5 layers E / Ad / T / Ad / E, T / Ad / E / Ad / T, Ad / E / Ad / E / Ad, T / Ad / E / Ad / E 6 layers T / Ad / E / Ad / E / Ad 7 layers T / Ad / E / Ad / E / Ad / T

[0060] The method for producing this multilayer molded article is not particularly limited. For example, there may be mentioned a method of melt-extruding another thermoplastic resin onto a molded article obtained from the resin composition of the present invention, a method of co-extruding the resin composition of the present invention and another thermoplastic resin, a method of coinjecting the resin composition of the present invention and another thermoplastic resin, and a method of laminating a molded article made of the resin composition of the present invention and a film or sheet of another substrate using a known adhesive such as an organic titanium compound, an isocyanate compound, or a polyester compound.

[0061] <Multi-layer pipe> The multi-layer pipe of the present invention has at least one layer made of the resin composition. The multi-layer pipe of the present invention has excellent gas barrier properties because the resin composition is mainly composed of EVOH (A), and in the first embodiment containing antioxidant (C), oxidative degradation of EVOH (A) at high temperatures is suppressed, so that the layer made of the resin composition is unlikely to suffer from deterioration in physical properties due to oxidative degradation even when used at high temperatures for a long period of time. Taking advantage of these properties, the multi-layer pipe of the present invention is suitably used as a hot water circulation pipe and a heat-insulated multi-layer pipe for district heating and cooling.

[0062] The layer structure of the multilayer pipe may be that of the multilayer molded article. When the multilayer pipe is used as a hot water circulating pipe, a three-layer structure of T / Ad / E, in which the layer made of the resin composition is the outermost layer, is generally adopted. A multilayer pipe of such a layer structure may be manufactured by adding a co-extrusion coating facility for the resin composition of the present invention and an adhesive resin to an existing manufacturing line for a single-layer pipe of crosslinked polyolefin or the like.

[0063] Providing polyolefin layers or the like on both sides of the layer made of the resin composition of the present invention and using the resin composition layers as intermediate layers is effective in preventing damage to the resin composition layer. On the other hand, when a multilayer pipe is used as a hot water circulation pipe, it is usually buried under a floor, so the risk of damage to the layer made of the resin composition of the present invention due to physical impact is relatively small, and therefore, from the viewpoint of prioritizing gas barrier properties, it is desirable to arrange the resin composition layer as the outermost layer. The gas barrier properties of EVOH (A) are humidity dependent, and the barrier properties decrease under high humidity conditions. Therefore, by making the layer made of the resin composition of the present invention mainly composed of EVOH (A) the outermost layer, the resin composition layer is arranged at the position farthest from the inner surface of the pipe that comes into contact with water, and the gas barrier performance is further improved. On the other hand, when an EVOH (A) layer is generally arranged as the outermost layer, it comes into direct contact with air and is therefore susceptible to oxidation deterioration. In such an environment, by disposing a layer made of the resin composition of the present invention, which is resistant to oxidative degradation even at high temperatures, as the outermost layer, delamination of the resulting multi-layer pipe is suppressed even when the resin composition is rapidly cooled after melt extrusion, and the effect of the present invention, that is, a multi-layer pipe having good gas barrier properties while suppressing the decrease in mechanical properties due to oxidative degradation, can be more effectively exerted.

[0064] <Method of manufacturing molded body and multi-layer pipe> A method for producing a multi-layer pipe will be described below, but part or all of this method can also be applied to other molded products (films, sheets, etc.).

[0065] The method for producing the multi-layer pipe of the present invention is not particularly limited, but examples thereof include (1) a method of producing the pipe by co-extrusion coating the resin composition of the present invention and an adhesive resin on a single-layer pipe such as a crosslinked polyolefin, and (2) a method of carrying out so-called co-extrusion molding, in which the number of extruders corresponding to the types of resin layers is used and the flows of molten resins in the extruders are simultaneously extruded in a layered state in which they are superimposed. In the case of (1), a molten film of the resin composition of the present invention and the adhesive resin can be simply coated on the single-layer pipe, but the adhesive strength between the pipe and the coating layer may be insufficient. As a countermeasure, the surface of the pipe to be coated before coating can be subjected to frame treatment and / or corona discharge treatment, which can suppress the deterioration of gas barrier properties caused by peeling of the coating layer during long-term use.

[0066] The method for producing a multilayer pipe preferably includes a step of cooling with water or air at 10 to 50 ° C. immediately after molding. That is, it is desirable to solidify the layer of the resin composition of the present invention by cooling with water or air at 10 to 50 ° C. before the layer of the resin composition of the present invention solidifies after melt molding. If the temperature of the water or air is too low, when the multilayer pipe is bent in the subsequent secondary processing step, cracks due to distortion tend to occur in the layer of the resin composition of the present invention at the bent portion. Although the details of the cause of the tendency of cracks due to distortion are not clear, it is presumed that residual stress in the molded product is the cause. From this viewpoint, the temperature of the water or air is more preferably 15 ° C. or higher, and more preferably 20 ° C. or higher. On the other hand, if the temperature of the water or air is too high, cracks due to distortion tend to occur in the layer of the resin composition of the present invention at the bent portion during secondary processing. Although the details of the cause of this have not been fully elucidated, it is presumed that the degree of crystallinity of the layer of the resin composition of the present invention becomes too high. From the above viewpoint, the temperature of the water or air is more preferably 40 ° C. or lower, and more preferably 30 ° C. or lower. The resin composition of the present invention is particularly applicable to the cooling process since, even when the resin composition is melt-extruded and then rapidly cooled in the manufacturing process of the multilayer pipe, the interlayer adhesion is not easily reduced and the resulting multilayer pipe is prevented from delaminating. The multilayer pipe thus obtained can be subjected to secondary processing to obtain multilayer pipes of various shapes. As the secondary processing method, a known secondary processing method can be appropriately used, and for example, a method of heating the multilayer pipe to 80 to 160°C, deforming it into a desired shape, and fixing it for 1 minute to 2 hours can be mentioned.

[0067] The multi-layer pipe of the present invention is preferably used, particularly for multi-layer pipes having a resin composition layer as the outermost layer, because delamination between layers is suppressed even when the EVOH resin composition is melt-extruded and then rapidly cooled during the production process, and the multi-layer pipe has excellent appearance properties and thermal stability. EXAMPLES

[0068] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The analyses and evaluations in the examples were carried out by the following methods.

[0069] (1) Ethylene unit content and degree of saponification of EVOH The resin compositions obtained in each of the Examples and Comparative Examples were dissolved in deuterated dimethyl sulfoxide (DMSO-d6) containing tetramethylsilane (TMS) as an internal standard substance and trifluoroacetic acid (TFA) as an additive, and were analyzed by a 500 MHz 1 Measurement was performed at 80° C. using H-NMR (JEOL Ltd., “GX-500”), and the ethylene unit content and degree of saponification were determined from the peak intensity ratio of ethylene units, vinyl alcohol units, and vinyl ester units.

[0070] (2) Content of metal ions, phosphate compounds, and boron compounds 0.5 g of the resin composition obtained in each Example and Comparative Example was placed in a Teflon (registered trademark) pressure vessel, and 5 mL of concentrated nitric acid was added thereto and decomposed at room temperature for 30 minutes. After decomposition, the vessel was covered and further decomposed by heating at 150°C for 10 minutes and then at 180°C for 5 minutes in a wet decomposition apparatus, and then cooled to room temperature. This treatment liquid was transferred to a 50 mL measuring flask and made up to 10 mL with pure water. The content of metal ions in the resin composition was quantified by measuring this solution using a PerkinElmer ICP emission spectrometer "Avio500". The content of phosphoric acid compounds and boron compounds can also be quantified by the same method.

[0071] (3) pH of hot water extract 10 g of the resin composition obtained in each of the Examples and Comparative Examples and 50 mL of pure water were placed in a 100 mL Erlenmeyer flask with a stopper, a cooling condenser was attached, and the mixture was stirred for 8 hours at 95° C. The resulting extract was cooled to 20° C., and then the pH was measured.

[0072] (4) Carboxylic acid content The carboxylic acid content of the extract obtained in (3) was quantified by titrating with 0.02 mol / L aqueous sodium hydroxide solution using phenolphthalein as an indicator.

[0073] (5)Yellowness (YI) The yellowness index (YI) of the resin compositions obtained in each of the Examples and Comparative Examples was measured using a spectrophotometer (LabScan XE Sensor manufactured by HunterLab) and was judged according to the following criteria: The YI value is an index that indicates the yellowness of an object, and the higher the YI value, the stronger the yellowness, whereas the lower the YI value, the weaker the yellowness and the less coloring. Judgment criteria A: Under 18 B: 18 to 21 C: 21 to 24 D: 24 to 27 E: 27 and above

[0074] (6) Interlayer adhesion Using the resin composition obtained in each Example and Comparative Example, linear low-density polyethylene ("Novatec LL-UF943" manufactured by Japan Polyethylene Co., Ltd., hereinafter abbreviated as LLDPE) and adhesive resin ("Binel CXA417E10" manufactured by DuPont diluted with the above LLDPE to 7% by mass, hereinafter abbreviated as Ad), a 3-kind 5-layer multilayer film (LLDPE / Ad / resin composition / Ad / LLDPE=50μm / 10μm / 10μm / 10μm / 50μm) was produced. The extruder, extrusion conditions, and die used were as follows: Extruder: Resin composition: Single screw extruder (TOYO SEIKI ME-type CO-EXT) Diameter 20mmφ, L / D20, full flight screw Feeding section / compression section / metering section / die=175 / 210 / 220 / 220℃ LLDPE: Single screw extruder (GT-32-A manufactured by the Institute of Plastics Engineering) Diameter 32mmφ, L / D28, full flight screw Feeding section / compression section / metering section / die=150 / 200 / 210 / 220℃ Ad: Single screw extruder (Technovel SZW20GT-20MG-STD) Diameter 20mmφ, L / D20, full flight screw Feeding section / compression section / metering section / die=150 / 200 / 220 / 220℃ Die: 300mm wide, 3 types, 5 layers coat hanger die (manufactured by the Institute of Plastics Engineering) Film take-up speed: 4m / min

[0075] The multilayer film extruded from the die was cooled by the following two methods. Slow cooling: The multilayer film discharged from the die was cooled by contacting it with a cooling roll at 70°C. Quenching: Immediately after being extruded from the die, the multilayer film was cooled by blowing 20°C compressed air (0.3 MPa) onto it from a distance of 1 cm, and then cooled by contacting it with a 70°C cooling roll.

[0076] For each condition, the multilayer film obtained 15 minutes after the start of film formation was conditioned at 23°C and 50% RH, and then a sample 150 mm long and 15 mm wide was cut along the extrusion direction. The peel strength was measured using a Shimadzu Corporation Autograph DCS-50M tensile tester at 23°C, 50% RH, and a T-peel mode at a tensile speed of 250 mm / min, and the peel strength was evaluated according to the following criteria. Judgment criteria A:550g / 15mm or more B: 500g / 15mm or more and less than 550g / 15mm C: 450g / 15mm or more and less than 500g / 15mm D: 400g / 15mm or more, less than 450g / 15mm E: Less than 400g / 15mm

[0077] (7) Thermal stability Using the resin compositions obtained in each of the Examples and Comparative Examples, a single-screw extruder (Toyo Seiki Seisakusho's "D2020", aperture 20 mmφ, L / D20) was used to obtain a single-layer film having a thickness of 100 μm under the following conditions. Screw diameter: 20mmφ (L / D=20, compression ratio=3.5, full flight type) Screw rotation speed: 100 rpm Extrusion temperature: feeding section / compression section / metering section / die = 180 / 220 / 220 / 250℃ Die: 300mm wide coat hanger die Take-up roll temperature: 80℃ Take-up speed: Approximately 1.5 m / min (adjust appropriately to achieve a thickness of 100 μm)

[0078] The obtained monolayer film was heat-treated at 150°C for a predetermined time in the atmosphere, and then conditioned at 23°C and 50% RH. A sample with a length of 150 mm and a width of 15 mm was cut along the extrusion direction, and the tensile elongation was measured at a tension speed of 250 mm / min in an atmosphere of 23°C and 50% RH using an autograph DCS-50M tensile tester manufactured by Shimadzu Corporation. Multiple samples were measured in the same manner except for changing the heat treatment time. Samples that were not heat-treated were also measured. The change in tensile elongation over time was evaluated from each measurement result, and the time at which the tensile elongation became 1 / 4 of that of the sample that was not heat-treated was determined, and the thermal stability was evaluated according to the following criteria. Judgment criteria A: More than 180 hours B: 150 hours or more but less than 180 hours C: 120 hours or more but less than 150 hours D: 90 hours or more but less than 120 hours E: Less than 90 hours

[0079] [Example 1] The hydrous EVOH pellets with an ethylene content of 32 mol%, a degree of saponification of 99.95 mol%, a melting point of 182°C, and a volatile content of 110 mass% were immersed in an aqueous solution containing potassium acetate, acetic acid, and phosphoric acid at 25°C for 6 hours and stirred. The concentrations of potassium acetate, acetic acid, and phosphoric acid in the aqueous solution in the immersion treatment were adjusted so that the contents in the resulting resin composition were as shown in Table 1. After the immersion treatment, the aqueous solution and the hydrous pellets were separated and dehydrated by centrifugal dehydration, and then placed in a hot air dryer and dried at 80°C for 3 hours and then at 110°C for 35 hours to reduce the volatile content to 0.3 mass% or less, thereby obtaining dried pellets. The volatile content of the hydrous EVOH pellets and the dried pellets was measured by gravimetry using a halogen moisture analyzer (Mettler Toledo "HX204") under the conditions of a drying temperature of 180°C, a drying time of 20 minutes, and a sample amount of 10 g.

[0080] Next, a hindered phenol-based antioxidant having an amide bond (BASF's "Irganox 1098", melting point 160°C, molecular weight 637) and sorbic acid (molecular weight 112) were added to the dried pellets, and the mixture was fed to a twin-screw extruder "TEX30α" (screw diameter 30 mm) manufactured by Japan Steel Works, Ltd., and melt-kneaded at a melt temperature of 220 to 230°C and an extrusion rate of 20 kg / hr using a screw having a forward shift kneading disk with a screw configuration of L (screw length) / D (screw diameter) = 3 to obtain a strand. The obtained strand was cooled and solidified in a cooling tank and then cut to obtain a resin composition of the present invention. The amounts of the hindered phenol-based antioxidant and sorbic acid added were adjusted so that the contents in the obtained resin composition were as shown in Table 1. The obtained resin composition was subjected to the above-mentioned various analyses and evaluations. The results are shown in Table 1.

[0081] [Example 2~ 3、6~12、14~ 17 、Reference Example 1 , Comparative Example 1~ 7 ] A resin composition was obtained in the same manner as in Example 1, except that the type and amount of each raw material were changed so that the composition of the obtained resin composition was as shown in Table 1. Various evaluations were performed on the obtained resin composition. The results are shown in Table 1. The resin composition obtained in Example 14 had excellent gas barrier properties compared to the resin composition obtained in Example 1, but on the other hand, the coloring resistance and thermal stability were decreased. In addition, the resin composition obtained in Example 15 had excellent coloring resistance and thermal stability compared to the resin composition obtained in Example 1, but on the other hand, the gas barrier properties were decreased.

[0082] [Table 1]

[0083] [Example 18] High density polyethylene (Novatec HD HE421 manufactured by Nippon Polyethylene Co., Ltd., density 0.956g / cc, MFR 0.14g / 10min (temperature 190°C, load 2160g)) was put into the first extruder, the resin composition obtained in Example 1 was put into the second extruder, and further, Admer NF518 manufactured by Mitsui Chemicals Inc. was put into the third extruder as an adhesive resin, and a multi-layer pipe having an outer diameter of 20mm was extruded using a three-kind three-layer circular die, and immediately after that, it was cooled and solidified through a cooling water tank adjusted to 40°C. The layer structure of the multi-layer pipe was a resin composition layer as the outermost layer, and the resin composition layer / adhesive resin layer / high density polyethylene layer = 100μm / 100μm / 2000μm. The obtained multi-layer pipe had excellent interlayer adhesion, gas barrier properties, appearance and thermal stability, and could be preferably used as a hot water circulation pipe.

Claims

1. A resin composition comprising an ethylene-vinyl alcohol copolymer (A), a potassium salt (B) and an antioxidant (C), The ethylene-vinyl alcohol copolymer (A) has an ethylene content of 15 to 60 mol % and a degree of saponification of 85 mol % or more; The potassium salt (B) is potassium acetate, the content of the potassium salt (B) relative to the ethylene-vinyl alcohol copolymer (A) is 200 to 1000 ppm in terms of potassium, the antioxidant (C) is a hindered phenol-based antioxidant having an ester bond or an amide bond, The content of the antioxidant (C) relative to 100 parts by mass of the ethylene-vinyl alcohol copolymer (A) is 0.1 to 4 parts by mass, A resin composition, in which 10 g of the resin composition is added to 50 ml of pure water and extracted at 95° C. for 8 hours, the extract has a pH of 5.05 to 5.5 at 20° C.

2. The resin composition according to claim 1, wherein a multilayer film having a layer made of the resin composition has an interlayer adhesive strength of 450 g / 15 mm or more as measured under evaluation conditions described in the examples.

3. Further containing a conjugated polyene compound (D), The resin composition according to claim 1 or 2, wherein the content of the conjugated polyene compound (D) is 0.001 to 0.15 parts by mass based on 100 parts by mass of the ethylene-vinyl alcohol copolymer (A).

4. A molded article having at least one layer made of the resin composition according to any one of claims 1 to 3.

5. A multi-layer pipe having at least one layer made of the resin composition according to any one of claims 1 to 3.

6. A multi-layer pipe having a layer made of the resin composition according to any one of claims 1 to 3 as an outermost layer.

7. A method for producing a multi-layer pipe having at least one layer made of the resin composition according to any one of claims 1 to 3, A method for producing a multi-layer pipe, comprising a step of cooling each layer constituting the multi-layer pipe with water or air at 10 to 50°C immediately after extrusion from a die.

Citation Information

Patent Citations

  • Resin composition

    JP1988286459A

  • Ethylene / vinyl alcohol copolymer composition

    JP1989069652A

  • Antioxidant ethylene / vinyl alcohol polymer composition

    JP1992227744A

  • Process for preparation of ethylene / Vinyl alcohol copolymer resin composition and process for preparation of resin pellet

    JP2001354779A

  • Method for producing ethylene-vinyl alcohol copolymer resin composition

    JP2006137957A