Rubber composition, its manufacturing method, and transmission belt

The rubber composition for power transmission belts, combining ethylene-α-olefin elastomer with specific silane coupling agents, addresses the challenge of achieving both heat resistance and abrasion resistance, enhancing durability and efficiency.

JP7571240B2Active Publication Date: 2024-10-22MITSUBOSHI BELTING LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023167730
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-28
Filing Date
2023-09-28
Publication Date
2024-10-22
Estimated Expiration
2040-06-18

AI Technical Summary

Technical Problem

Existing power transmission belts face challenges in achieving a high degree of compatibility between heat resistance and abrasion resistance, which are critical for durability and transmission efficiency.

Method used

A rubber composition comprising ethylene-α-olefin elastomer, organic peroxide, silica, a silane coupling agent with ethylenically unsaturated bonds, and a silane coupling agent with a sulfur atom, optimized by adjusting the blending ratios and specific surface area of silica, molecular weight, and number of silicon atoms, to enhance heat resistance and abrasion resistance.

Benefits of technology

The composition achieves both high heat resistance and abrasion resistance, improving durability and maintaining transmission efficiency by reducing internal heat generation and crack formation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571240000007
    Figure 0007571240000007
  • Figure 0007571240000008
    Figure 0007571240000008
  • Figure 0007571240000009
    Figure 0007571240000009
Patent Text Reader

Abstract

To provide a rubber composition capable of achieving both heat resistance and abrasion resistance.SOLUTION: There is prepared a rubber composition by a production method comprising a first kneading step of combining an ethylene-α-olefin elastomer (A), an organic peroxide (B), silica (C), a silane coupling agent containing an ethylenically unsaturated bond (D) and a silane coupling agent containing a sulfur atom (E) and kneading the component containing the silica (C) at a kneading temperature of 150°C or more and a second kneading step of kneading the component containing the silane coupling agent (E) containing a sulfur atom at a kneading temperature of 120°C or less. A transmission belt may be prepared by forming a transmission surface by the rubber composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition for forming a transmission surface of a transmission belt, a method for producing the same, and The present invention relates to a power transmission belt having a power transmission surface formed from the rubber composition. [Background technology]

[0002] Conventionally, the transmission belts used in the fields of automobiles and motorcycles have a long service life (durability The deterioration that determines the durability of a transmission belt is the thermal deterioration of the rubber layer. These include cracks caused by oxidation and wear on the contact surface with the pulley. From the viewpoint of using a rubber composition having such properties, a transmission belt having excellent durability has been provided. Regarding the rubber properties, rubber components that do not contain double bonds in the main chain are adopted, and in particular, EPDM (ethylenediaminetetraacetate) Ethylene-α-olefin elastomers, such as ethylene-propylene-diene terpolymers The number of power transmission belts using EPDM as the rubber component is increasing. The content of diene components (components with double bonds in the side chain) introduced as crosslinking points is small. The high-temperature grade is preferably used as a rubber component having excellent heat resistance. In rubber components with as few double bonds as possible, cross-linking with sulfur is not possible, so Organic peroxides are used for this purpose.

[0003] On the other hand, ethylene-α-olefin elastomers do not have polar groups, so It is a rubber component that can be highly filled with reinforcing agents such as carbon black, silica, and short fibers, and the rubber composition It is also used to increase the hardness and modulus of the material. Carbon black is widely used, but adding a large amount of it increases the self-heating of the rubber composition. In consideration of this drawback, it is recommended to use it as a reinforcing agent. Although a method using silica is also known, when a large amount of silica is added, the rubber composition The increase in viscosity reduces the kneadability and the dispersibility of silica. Therefore, a silane coupling agent is usually added to the rubber composition. By improving the dispersion of silica in the material, it is possible to develop a transmission bearing that is both heat-resistant and wear-resistant. A route has been provided.

[0004] In Japanese Patent Laid-Open No. 2006-275191 (Patent Document 1), the transmission surface is made of EPDM and organic peroxide. A rubber composition containing a vinyl silane compound having a boiling point of 150 to 350°C. This document discloses a friction transmission belt made of a material containing a vinyl-based silane. This improves processability and cross-linked strength, and also provides excellent abrasion resistance and durability. It is shown that:

[0005] In Japanese Patent Laid-Open Publication No. 2006-194322 (Patent Document 2), EPDM, short fibers, and silica are used. A friction transmission belt comprising a compressed rubber layer having a single layer structure is disclosed. This document states that the inclusion of silica increases rigidity and makes the material more susceptible to cracking, but It is described that the inclusion of a coupling agent can suppress the occurrence of cracks. is.

[0006] In JP 2011-252510 A (Patent Document 3), the compression rubber layer is made of EPDM, Friction transmission bell made of rubber compound containing rubber, short fiber, and silane coupling agent This document discloses that the incorporation of a silane coupling agent results in a silane-coated It is also disclosed that this improves the dispersibility of silica and improves the adhesive strength between silica and rubber. It is described as being effective in improving transmission performance and wear resistance in water.

[0007] In Japanese Patent Laid-Open No. 10-182885 (Patent Document 4), silica, alkoxysilane and and a sulfur-containing silane coupling agent. It is described that the processability of the rubber compounded composition is improved without impairing the heat resistance and abrasion resistance. In the examples, the rubber is a sulfur-crosslinked diene rubber, a natural rubber, a styrene rubber, etc. Styrene-butadiene copolymer rubber (SBR) is used. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2006-275191 A (Claim 1, paragraph

[0011] ) [Patent Document 2] JP 2006-194322 A (Claim 1, paragraph

[0026] ) [Patent Document 3] JP 2011-252510 A (claims 1 and 3, paragraph

[0037] ) [Patent Document 4] JP-A-10-182885 (Claim 1, paragraph

[0004] , Examples) Summary of the Invention [Problem to be solved by the invention]

[0009] In recent years, there has been a strong demand for improved heat resistance in power transmission belts. V-ribbed belts used in drive systems and variable speed belts used in continuously variable transmissions in motorcycles (Ro Even in belts such as 1-edge V-belts, the two main factors in durability are high heat resistance and abrasion resistance. However, the rubber compositions of Patent Documents 1 to 4 have poor heat resistance and abrasion resistance. It was not possible to achieve a high level of compatibility.

[0010] The object of the present invention is to provide a rubber composition and a method for producing the same that can achieve both heat resistance and abrasion resistance. Another object of the present invention is to provide a power transmission belt having a power transmission surface formed from the rubber composition.

[0011] Another object of the present invention is to provide a power transmission belt which is excellent in both heat resistance and abrasion resistance and has excellent durability. The purpose of this invention is to provide

[0012] It is still another object of the present invention to provide a power transmission belt having high durability and transmission efficiency. be. [Means for solving the problem]

[0013] As a result of extensive research into achieving the above object, the present inventors have discovered that an ethylene-α-olefin ethylene copolymer is A polymer consisting of elastomer (A), organic peroxide (B), silica (C), and an ethylenically unsaturated bond. Silane coupling agent (D) containing a sulfur atom and silane coupling agent (E ) can provide both heat resistance and wear resistance. ), the compounding ratio of the silane coupling agents (D) and (E), the number of silicon atoms (silyl groups), By adjusting the specific surface area and molecular weight within a specific range, high heat resistance and abrasion resistance are achieved. The inventors have found that it is possible to improve the durability of the power transmission belt while maintaining the above-mentioned properties, and have completed the present invention.

[0014] That is, the rubber composition of the present invention comprises an ethylene-α-olefin elastomer (A), Organic peroxide (B), silica (C), silane coupling agent containing ethylenically unsaturated bonds The silane coupling agent (D) and the silane coupling agent (E) containing a sulfur atom are included. The calculated value of X in the coupling agent (D) represented by the following formula (1) is X1, When the calculated value of X represented by the following formula (1) in the blocking agent (E) is X2, X1 and X The sum of 2 may be between 0.0001 and 0.0003.

[0015] X = a × [b / (c × d)] (1) (In the formula, a represents the ratio of the silane coupling agent to 100 parts by mass of silica, and b represents the ratio of the silane coupling agent to 100 parts by mass of silica.) is the number of silicon atoms in the silane coupling agent, c is the BET specific surface area of ​​silica, and d is (Indicates the molecular weight of the silane coupling agent)

[0016] The calculated value of Y in the silane coupling agent (D) represented by the following formula (2) is Y1, When the calculated value of Y in the silane coupling agent (E) represented by the following formula (2) is Y2, The ratio of Y1 to Y2 (Y1 / Y2) may be 0.8 to 6.

[0017] Y = a × (b / d) (2) (wherein a, b and d are the same as above)

[0018] The diene content of the ethylene-α-olefin elastomer (A) is 7% by mass or less. The ratio of the silica (C) may be 1:1 of the ethylene-α-olefin elastomer (A). The ratio of the organic peroxide (B) may be 25 to 120 parts by mass relative to 0.00 parts by mass. is 1 to 8 parts by mass relative to 100 parts by mass of the ethylene-α-olefin elastomer (A). The rubber composition may be used to form a power transmission surface of a power transmission belt.

[0019] The present invention includes an ethylene-α-olefin elastomer (A), an organic peroxide (B), (C), a silane coupling agent containing an ethylenically unsaturated bond (D) and a sulfur atom The method for producing the rubber composition further comprises heating and kneading a silane coupling agent (E) containing an alkyl group. Also included.

[0020] The present invention also includes a power transmission belt having a power transmission surface formed of a cured product of the rubber composition.

[0021] In the present specification and claims, the term "(meth)acryloyl group" refers to an acryloyl group. The term "acryloyl" refers to an acryloyl group and a methacryloyl group. Effect of the Invention

[0022] In the present invention, an ethylene-α-olefin elastomer (A), an organic peroxide (B), and (C) silica, (D) a silane coupling agent containing an ethylenically unsaturated bond, and (E) a sulfur It is combined with a silane coupling agent (E) containing sulfur atoms, so it has heat resistance and wear resistance. In particular, the silica (C), the silane coupling agent (D) and The compounding ratio of (E), the specific surface area of ​​the silica, the number of silicon atoms of the silane coupling agent, and By adjusting the molecular weight and heat resistance, which determine the durability of the material, The rubber composition of the present invention can achieve a high degree of compatibility and improve the durability of the power transmission belt. Since it contains silica as the main component of the reinforcing agent, when it is used to form the transmission surface of a transmission belt, it improves transmission efficiency. This maintains the strength while also improving durability. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 is a schematic diagram showing the layout of the wear resistance test of the V-ribbed belt obtained in the example. [Diagram 2] FIG. 2 is a schematic diagram showing the layout of the durability running test. [Diagram 3] FIG. 3 is a schematic diagram showing the layout of a biaxial running test for measuring the transmission loss of the V-ribbed belt obtained in the example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] [(A) Ethylene-α-olefin elastomer] The rubber composition (curable rubber composition) of the present invention contains ethylene-α-olefin as the rubber component. The ethylene-α-olefin elastomer (A) is a main chain It has excellent heat resistance because it does not contain double bonds (ethylenically unsaturated bonds).

[0025] The ethylene-α-olefin elastomer (A) contains, as structural units, an ethylene unit, an α It is sufficient that the compound contains an olefin unit, and may further contain a diene unit. The ethylene-α-olefin elastomer (A) is an ethylene-α-olefin copolymer. These include solid rubber, ethylene-α-olefin-diene terpolymer rubber, etc.

[0026] Examples of the α-olefins for forming the α-olefin units include propylene, Chain α-C such as butene, pentene, methylpentene, hexene, and octene 3-12 Me Among these α-olefins, α-C such as propylene 3- 4 Olefins, especially propylene, are preferred.

[0027] As the diene monomer for forming the diene unit, a non-conjugated diene monomer is usually used. Examples of non-conjugated diene monomers include dicyclopentadiene, methylene Norbornene, ethylidene norbornene, 1,4-hexadiene, cyclooctadiene, etc. Among these diene monomers, ethylidene norbornene, 1,4-hexene, Of these, norbornene (especially ethylidene norbornene) is preferred.

[0028] Representative ethylene-α-olefin elastomers include, for example, ethylene-propylene. Ethylene copolymer (EPM), ethylene-propylene-diene terpolymer (EPDM), etc. Examples include:

[0029] These ethylene-α-olefin elastomers may be used alone or in combination. Among these, ethylene-α- -Olefin-diene terpolymer rubber is preferred, and ethylene-propylene-diene copolymer is preferred. Copolymers (EPDM) are particularly preferred.

[0030] The ratio of ethylene to propylene in ethylene-propylene-diene terpolymers (mass ratio) is the former / the latter = 40 / 60 to 90 / 10, preferably 45 / 55 to 85 / 1 5 (for example, 50 / 50 to 82 / 18), more preferably 55 / 45 to 80 / 20 (especially The ratio may be about 55 / 45 to 75 / 25.

[0031] Ethylene-α-olefin elastomer (A) [especially ethylene-α-olefin elastomer such as EPDM] The diene content of the olefin-diene terpolymer rubber is 10% by mass or less (for example, 0.1 to 10% by mass), preferably 7% by mass or less (for example, 1 to 7% by mass), and Preferably, it is 6% by mass or less (e.g., 1.5 to 6% by mass), and most preferably, it is 5% by mass or less (e.g., For example, the diene content is 1.8 to 5% by mass. The diene content is excellent in various properties (particularly, transmission efficiency). From this viewpoint, for example, 2 to 7 mass%, preferably 3 to 6 mass%, and more preferably 3.5 to 5. The diene content is preferably 5% by mass, and most preferably 4 to 5% by mass. In applications where the physical properties of the crosslinked rubber are important, for example, 1 to 5 mass%, preferably 1.2 to 4 mass%, The content may be more preferably 1.5 to 3 mass %, and even more preferably 1.6 to 2 mass %. In the present invention, the heat resistance is improved by using a rubber component that does not have a double bond in the main chain. However, by limiting the amount of double bonds due to the diene units introduced as side chains, If the diene content is too high, there is a risk that high heat resistance cannot be guaranteed. be.

[0032] In the present specification and claims, the diene content is defined as ethylene-α-olefin. It means the mass ratio of diene monomer units in all units constituting the diene elastomer, and is conventionally used It can be measured by a method, but it may be a monomer ratio.

[0033] The proportion of ethylene-α-olefin elastomer (A) in the rubber component is 50 mass% or more. It is sufficient, preferably 80% by mass or more, more preferably 90% by mass or more, and most preferably Preferably, it is 100% by mass (ethylene-α-olefin elastomer only). If the ratio of the ethylene-α-olefin elastomer (A) in the polymer is too low, the heat resistance and There is a risk that the cold resistance may decrease.

[0034] [(B) Organic peroxide] In the present invention, the rubber component is an ethylene-α-olefin copolymer having a small number of double bonds that serve as crosslinking points. Since a polyvinyl elastomer (A) is used, an organic peroxide (B) is used as a crosslinking agent.

[0035] As the organic peroxide (B), a conventional component such as diacyl peroxide (diacyl peroxide) can be used. peroxide, dibenzoyl peroxide, etc.), peroxyketals (1, 1-Di(t-butylperoxy)cyclohexane, 2,2-Di(t-butylperoxy) butane, etc.), alkyl peroxy esters (t-butyl peroxybenzoate, etc.) , dialkyl peroxide (di-t-butyl peroxide, dicumyl peroxide , t-Butylcumyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxide) 2,5-Dimethyl-2,5-di(t-butylperoxy)hexyne-3 , 1,1-di(t-butylperoxy)-3,3,5-trimethylcyclohexane, 1, 3-Bis(2-t-butylperoxyisopropyl)benzene, 2,5-dimethyl-2 ,5-di(benzoylperoxy)hexane, etc.), peroxycarbonate (t-butyl butylperoxyisopropyl carbonate, t-butylperoxy-2-ethyl-hexyl Carbonate, t-amylperoxy-2-ethyl-hexyl carbonate, etc. Some examples include:

[0036] These organic peroxides can be used alone or in combination. Among these, dialkyl peroxides such as dicumyl peroxide are widely used.

[0037] The ratio of organic peroxide (B) is 100% by mass of ethylene-α-olefin elastomer (A). For example, 0.5 to 10 parts by mass, preferably 1 to 8 parts by mass, and more preferably The ratio of the organic peroxide (B) is preferably 2 to 7 parts by mass, and more preferably 3 to 6 parts by mass. If the amount is too large, the heat resistance and abrasion resistance of the rubber composition may decrease. The heat resistance and abrasion resistance of the composition may decrease.

[0038] [(C) Silica] The rubber composition of the present invention contains silica (C) as a reinforcing agent. Silica acts as a reinforcing agent for rubber. Compared to carbon black, which is widely used as a heat source, it generates less internal heat and is advantageous in terms of transmission loss. Therefore, the rubber composition of the present invention preferably contains silica as a main component of the reinforcing agent.

[0039] Silica (C) includes dry silica, wet silica, surface-treated silica, etc. Silica is classified into various types according to the manufacturing method, for example, dry process white carbon, wet process white carbon, etc. Silica can also be classified as silica, colloidal silica, precipitated silica, etc. Among these silicas, those having surface silanol groups are Silica (anhydrous silicic acid, hydrous silicic acid) is preferred, and hydrous silicic acid with many surface silanol groups is preferred. It has a strong chemical bond with rubber components.

[0040] The average particle size (average primary particle size) of the silica (C) is, for example, 1 to 500 nm, preferably 3 〜300nm, more preferably 5〜100nm, most preferably 10〜50nm If the particle size of the silica is too large, the reinforcing effect of the belt body may decrease, and if it is too small, , it may be difficult to disperse the particles uniformly.

[0041] In the present specification and claims, the average particle size of silica is measured by For example, the measurement can be performed using a transmission electron microscope.

[0042] The BET nitrogen adsorption specific surface area of ​​silica (C) is, for example, 50 to 400 m 2 / g, good Preferably 70~350m 2 / g, more preferably 100 to 300m 2 / g, more preferred Approximately 150~250m 2 The specific surface area can be selected depending on the application, for example, 7 0~300m 2 / g, preferably 100 to 250 m 2 / g, more preferably 150 to 2 00m 2 / g, and in applications where abrasion resistance is important, for example, 100 to 400 m 2 / g, preferably 150-300m 2 / g, more preferably 200 to 250 m 2 / g If the specific surface area is too large, transmission loss is likely to occur and the particles are not uniformly dispersed. If the specific surface area is too small, the reinforcing effect on the rubber component decreases. There is a risk that this may happen.

[0043] The ratio of silica (C) to 100 parts by mass of ethylene-α-olefin elastomer (A) is For example, 25 to 200 parts by mass, preferably 30 to 150 parts by mass, and more preferably The ratio is 40 to 100 parts by mass. The ratio is preferably ethylene-α-olefin because it has excellent properties. For example, 25 to 120 parts by mass, preferably 30 to 100 parts by mass, more preferably 35 to 80 parts by mass, and most preferably 40 to 60 parts by mass. In addition, the above ratio is preferably ethylene-α-olefin in applications where wear resistance is important. For example, 50 to 200 parts by mass, preferably 70 The silica (C) may be in the range of 80 to 150 parts by mass, and more preferably 80 to 120 parts by mass. If the ratio is too low, the reinforcing effect on the rubber may decrease, whereas if the ratio is too high, the abrasion resistance may decrease. There is a risk that the performance may decrease.

[0044] The proportion of silica (C) in the reinforcing agent may be 50% by mass or more, and preferably 80% by mass or more. % or more, more preferably 90% by mass or more, and most preferably 100% by mass (ethylene The proportion of silica (C) in the rubber component is small. If the thickness is too large, when the rubber composition is used to form a transmission surface of a transmission belt, the transmission efficiency may decrease. In particular, carbon black is widely used as a reinforcing agent for the rubber that forms the transmission surface of the transmission belt. However, if the proportion of carbon black as a reinforcing agent increases, internal generation in the rubber composition increases. This may result in increased heat and increased transmission loss.

[0045] [(D) Silane coupling agent containing an ethylenically unsaturated bond] The rubber composition of the present invention is characterized in that it enhances the dispersibility of the silica (C) in the rubber composition and improves abrasion resistance. As a silane coupling agent, it is used to improve the properties of ethylenically unsaturated bonds (double bonds). The silane coupling agent (D) contains:

[0046] In the silane coupling agent (D) containing a double bond, the ethylenically unsaturated bond is Examples of the groups include vinyl groups, allyl groups, (meth)acryloyl groups, and maleyl groups (maleic acid groups). Of these ethylenically unsaturated bonds, vinyl groups are , allyl groups, (meth)acryloyl groups, etc. are commonly used.

[0047] Examples of the vinyl group-containing silane coupling agent include vinyltrimethoxysilane, Vinyltriethoxysilane, vinyltriisopropoxysilane, etc. 1-4 a vinyltriacetoxysilane and other vinyltriacyloxysilanes; and vinyltrihalosilanes such as methyltrichlorosilane.

[0048] Examples of the allyl group-containing silane coupling agent include allylsilane; allyltrimethy Allyl tri-C such as xysilane 1-4 Alkoxysilanes; diallyldimethoxysilane, etc. Diaryl C 1-4 Alkoxysilanes; allyltrimethylsilane, etc. 1 -4 Alkylsilanes; diallyldi-C such as diallyldimethylsilane 1-4 Alkylsilane etc.

[0049] Examples of the (meth)acryloyl group-containing silane coupling agent include 2-(meth)acryloyl Acryloxyethyltrimethoxysilane, 2-(meth)acryloxyethyltriethoxysilane Lan, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane (Meth)acryloxy C such as dipropyltriethoxysilane 2-4 Alkyltri C 1- 2 Alkoxysilane; 3-(meth)acryloxypropylmethyldimethoxysilane, 3- (Meth)acryloxy C such as (meth)acryloxypropylmethyldiethoxysilane 2 -4 Alkyl-C 1-4 Alkyl-diC 1-4Alkoxysilanes and the like.

[0050] These silane coupling agents can be used alone or in combination. Among these, (meth)acryloyl group-containing silane coupling agents are preferred, and (meth)acryloyl Cryloxy C 2-4 Alkyltri C 1-2 Alkoxysilanes are particularly preferred.

[0051] The number of silicon atoms in the molecule of the silane coupling agent (D) may be 1 or more. For example, it can be selected from the range of about 1 to 15, preferably 1 to 12, and more preferably 1 to The number of silicon atoms is preferably 1 to 10, and more preferably 1 to 8. The number of silicon atoms can be appropriately selected depending on the application. For example, it is 1 to 5, preferably 1 to 3, more preferably 1 to 2, and even more preferably 1. This is also fine.

[0052] The molecular weight of the silane coupling agent (D) is selected, for example, from the range of about 100 to 3000. For example, it can be 120 to 2000, preferably 150 to 1500, and more preferably 180 The molecular weight is preferably from 200 to 800, and more preferably from 200 to 800. The molecular weight is appropriately selected depending on the application. For example, the range can be selected from 100 to 500, preferably from 150 to 400, and more preferably from 180 to 300, and more preferably 200-250.

[0053] The ratio of the silane coupling agent (D) to 100 parts by mass of the silica (B) is, for example, 1 up to 20 parts by mass, preferably 1.5 to 10 parts by mass, more preferably 2 to 8 parts by mass, and most preferably The amount of the silane coupling agent relative to the silica (B) is preferably 3 to 7 parts by mass. The ratio of (D) is the ratio of silica (B) and silane coupling agent (E) containing a sulfur atom. is selected from such a range so that the relationship is within a specific range defined by X and Y. It is preferable to adjust the temperature by

[0054] [(E) Silane coupling agent containing a sulfur atom] The rubber composition of the present invention is provided with a silane coupling agent having an ethylenically unsaturated bond. In addition to the silane coupling agent, a silane coupling agent (E) containing a sulfur atom is further added. Conventionally, peroxide crosslinking rubber compositions using organic peroxides as crosslinking agents have been used. Silane coupling agents are used in rubber compositions with few double bonds, such as EPDM. In addition, silane coupling agents containing sulfur atoms are less effective in improving wear resistance. In contrast, in the present invention, a silane coupling agent containing a sulfur atom is used. The coupling agent (E) is combined with silica (C) and a silane coupling agent (D) containing a double bond. By combining these, it is possible to achieve both wear resistance and heat resistance. The silane coupling agent is added to improve the dispersibility of silica and ensure abrasion resistance. Therefore, it was unexpected that the silane coupling agent (E) contributes to heat resistance. .

[0055] In addition, in a rubber composition, as a means for improving heat resistance, the amount of an antioxidant is increased. However, this conventional method tends to increase internal heat generation in the rubber composition. This increases the transmission loss (decreases the transmission efficiency) and reduces the fuel efficiency. By combining different types of silane coupling agents, the decrease in transmission efficiency is also suppressed. While maintaining the above properties, it is possible to achieve both heat resistance and abrasion resistance.

[0056] The sulfur-containing silane coupling agent (E) is a mercapto group-containing silane coupling agent. Coupling agents, disulfide group-containing silane coupling agents, tetrasulfide group-containing silane coupling agents coupling agents, etc., include silane coupling agents containing di- or tetrasulfide groups. do.

[0057] Examples of mercapto group-containing silane coupling agents include 3-mercaptopropyl silane. mercapto C such as trimethoxysilane and 3-mercaptopropyltriethoxysilane 2- 4 Alkyltri C 1-4 Alkoxysilane; 3-Mercaptopropylmethyldimethoxysilane Mercapto C of orchids, etc. 2-4 Alkyl-C 1-4 Alkyl-diC 1-4 Alkoxysilane Examples include

[0058] Examples of disulfide group-containing silane coupling agents include bis(3-(trimethoxysilane) Bis(3-(triethoxysilyl)propyl)disulfide, Bis(3-(triethoxysilyl)propyl)disulfide Bis(TriC) such as Rufido 1-4 Alkoxysilyl-C 2-4 (alkyl) disulfide etc.

[0059] Examples of tetrasulfide group-containing silane coupling agents include bis[3-(trimethylsilyl) bis[3-(triethoxysilyl)-propyl]tetrasulfide, Bis(trimethylsilyl)tetrasulfide etc. 1-4 Alkoxysilyl-C 2-4 Alki tetrasulfide, etc.

[0060] These silane coupling agents can be used alone or in combination. Among these, silane coupling agents containing di- or tetrasulfide groups are preferred, and disulfide groups are preferred. Silane coupling agents containing a silane group are more preferred, and bis(triC 1-4 Alkoxysilane Ru-C 2-4 Alkyl) disulfides are particularly preferred.

[0061] The number of silicon atoms (silyl groups) in the molecule of the silane coupling agent (E) is 1 or more. For example, 1 to 10, preferably 1 to 5, more preferably 2 to 3, and most preferably Most likely it is 2.

[0062] The molecular weight of the silane coupling agent (E) is, for example, 100 to 1000, preferably 200. 〜800, more preferably 300〜600, even more preferably 400〜550, most preferably Usually it is 400 to 500.

[0063] The ratio of the silane coupling agent (E) to 100 parts by mass of the silica (B) is, for example, 0. 0.1 to 20 parts by weight, preferably 0.3 to 10 parts by weight, and more preferably 0.5 to 8 parts by weight and most preferably 1 to 6 parts by mass. In the present invention, the ratio of the silane cap to the silica (B) is The ratio of the coupling agent (E) is the ratio of silica (B) and the silane coupling agent containing the double bond. The relationship between the compound (D) and the blocking agent (C) is determined so as to be within a specific range defined by the above X and Y. It is preferable to select and adjust from a range.

[0064] Short Fiber (F) The rubber composition of the present invention may further contain short fibers (F). For example, natural staple fibers (such as cotton and other natural cellulosic staple fibers), semi-synthetic staple fibers (such as lace Semi-synthetic cellulosic staple fibers such as cellulose acetate, polyester staple fibers (polyethylene terephthalate, etc.) Polyalkylene arylate staple fibers, etc.), polyamide staple fibers (nylon (Nylon 66 staple fiber, aliphatic polyamide staple fiber such as nylon 66 staple fiber, aramid staple fiber, etc.) Some examples include:

[0065] These short fibers can be used alone or in combination of two or more. Polyester staple fibers and polyamide staple fibers are commonly used, and aliphatic polyamide fibers are preferred.

[0066] The average fiber length of the short fibers is, for example, 0.1 to 30 mm, preferably 0.2 to 20 mm, and more preferably 0.1 to 30 mm. The thickness is preferably 0.3 to 15 mm, and most preferably 0.5 to 5 mm.

[0067] These short fibers can be optionally treated with surfactants, silane coupling agents, epoxy compounds, etc. The surface may be treated with a compound such as an isocyanate compound.

[0068] The short fibers are used to improve adhesion with the ethylene-α-olefin elastomer (A). If necessary, an adhesive treatment may be applied. As the adhesive treatment, a conventional adhesive treatment may be used. For example, adhesive components [e.g., epoxy compounds, isocyanate compounds] are dissolved in an organic solvent. Immersion in resin-based treatment liquids (toluene, xylene, methyl ethyl ketone, etc.) Immersion treatment, immersion treatment in resorcinol-formalin-latex liquid (RFL liquid), rubber composition One example is a dipping treatment in rubber cement prepared by dissolving the above in an organic solvent.

[0069] The proportion of short fiber (F) is ethylene-α-olefin to further reduce torque loss. For example, 1 to 100 parts by mass, preferably 5 parts by mass, based on 100 parts by mass of the copolymer elastomer (A). up to 80 parts by mass, more preferably 10 to 50 parts by mass, and most preferably 20 to 40 parts by mass. If the proportion of short fibers is too low, the effect of improving heat resistance and abrasion resistance may decrease. On the other hand, if the amount is too large, the transmission efficiency may decrease.

[0070] [Other ingredients] The rubber composition of the present invention contains, as a rubber component, an ethylene-α-olefin elastomer (A In addition to the above, other rubber components may be further included. Examples of the other rubber components include Diene rubber (natural rubber, isoprene rubber, butadiene rubber, chloroprene rubber, styrene SBR, acrylonitrile butadiene rubber (nitrile rubber), hydrogen nitrile rubber, chlorosulfonated polyethylene rubber, alkylated chlorosulfone Polyethylene rubber, epichlorohydrin rubber, acrylic rubber, silicone rubber, urea These other rubber components may be used alone or in combination. Can be used in combination.

[0071] Other rubber components are, relative to 100 parts by mass of ethylene-α-olefin elastomer (A): It may be 100 parts by mass or less (for example, about 0.1 to 100 parts by mass), and preferably 25 parts by mass or less, and more preferably 10 parts by mass or less.

[0072] The rubber composition of the present invention further contains, as a reinforcing agent, another reinforcing agent in addition to the silica (C). Other reinforcing agents include, for example, carbon black, clay, calcium carbonate, etc. These reinforcing agents may be used alone or in combination of two or more. Can be used in combination.

[0073] The ratio of other reinforcing agents is 100 parts by mass or less (for example, 0.01 parts by mass) per 100 parts by mass of silica (C). The amount may be about 1 to 100 parts by mass, preferably 50 parts by mass or less, and more preferably is preferably 30 parts by mass or less, and most preferably 10 parts by mass or less.

[0074] The rubber composition of the present invention contains the silane coupling agent (D In addition to (A) and (B), other silane coupling agents may be further included.

[0075] Other silane coupling agents include, for example, alkoxysilyl group-containing silane coupling agents. coupling agents, halogen-containing silane coupling agents, epoxy-containing silane coupling agents, Amino group-containing silane coupling agents, carboxyl group-containing silane coupling agents, silano These silane coupling agents include silane coupling agents containing a silane group. They can be used alone or in combination of two or more.

[0076] The ratio of other silane coupling agents is the total of silane coupling agents (D) and (E). Even if it is less than 100 parts by mass (for example, about 0.1 to 100 parts by mass) Preferably, the amount is 50 parts by mass or less, more preferably 30 parts by mass or less, and most preferably 1 0 parts by mass or less.

[0077] The rubber composition of the present invention further contains conventional additives that are used as compounding agents for rubber. Examples of conventional additives include co-crosslinking agents (such as bismaleimides), vulcanization aids, etc. vulcanization accelerators (such as thiuram accelerators), vulcanization retarders, metal oxides (zinc oxide, acid Magnesium oxide, calcium oxide, barium oxide, iron oxide, copper oxide, titanium oxide, aluminum oxide Aluminum, etc.), softeners (paraffin oil, naphthenic oil, etc.) , processing agents or processing aids (stearic acid, metal stearates, waxes, paraffins, Fatty acid amides, etc.), anti-aging agents (antioxidants, heat anti-aging agents, flex crack prevention agents, ozone Deterioration inhibitors, colorants, tackifiers, stabilizers (UV absorbers, heat stabilizers, etc.), These additives may be used alone or in combination of two or more. The metal oxide may also act as a crosslinking agent.

[0078] The total proportion of conventional additives is 100 mass % of ethylene-α-olefin elastomer (A). For example, 5 to 50 parts by mass, preferably 10 to 30 parts by mass, and more preferably 1 The content is 5 to 25 parts by mass.

[0079] [Characteristics of rubber composition] The rubber composition of the present invention comprises a silane coupling agent (D) containing a double bond and a sulfur atom. The present invention is characterized by combining a silane coupling agent (E) containing a silane. As a coupling agent, in the peroxide crosslinking rubber composition, a silyl group containing a double bond is used. In the case of a sulfur-crosslinked rubber composition, a sulfur-containing silane coupling agent is used. In contrast, in the present invention, a peroxy coupling agent is used. In a side crosslinking rubber composition, the combination of the two improves heat resistance and abrasion resistance. made it possible to achieve both.

[0080] The ratio of the silane coupling agent (E) to 100 parts by mass of the silane coupling agent (D) is For example, 5 to 300 parts by mass, preferably 10 to 200 parts by mass, and more preferably 15 to 300 parts by mass. The amount of the silane coupling agent (E If the proportion of the silane coupling agent (E) is too high, the abrasion resistance may decrease. If the amount is too small, the heat resistance may decrease.

[0081] Further, as described above, the rubber composition of the present invention further comprises the silica (C), the silane cuprate (B), and the like. The compounding ratio of the silane coupling agents (D) and (E), the specific surface area of ​​the silica, The number of silicon atoms and the molecular weight of the agent are adjusted to a specific range, and the sum of X1 and X2 and By controlling the Y1 / Y2 ratio, it is possible to improve the heat resistance and abrasion resistance, which affect the durability of the steel. It is possible to achieve both at the same time.

[0082] The total value of X1 and X2 is, for example, 0.0001 to 0.0003, preferably 0. 00012 to 0.00028, more preferably 0.00013 to 0.00025, and most preferably The total value is preferably 0.00014 to 0.00024. If the total value is too small, the heat resistance Conversely, if it is too large, it may be difficult to achieve both heat resistance and wear resistance. It becomes difficult to balance wear resistance and durability, and the processability and economy are also reduced. There is a risk.

[0083] The Y1 / Y2 ratio is, for example, 0.8 to 6, preferably 0.9 to 5.5, and more preferably The Y1 / Y2 ratio is preferably 1 to 5, and more preferably 1 to 4.8. If the Y1 / Y2 ratio is too small, the abrasion resistance If it is too large, the transmission efficiency of the belt may decrease. There is a risk that the durability will decrease when used in a car.

[0084] The cured product (crosslinked product) of the rubber composition of the present invention has a low internal loss tangent (tan δ). The loss tangent (tan δ) is the ratio of the loss modulus (E") to the storage modulus (E'). It can be calculated by dividing by the amount of heat dissipated during one vibration cycle. It is expressed as the ratio of the energy lost to the maximum energy stored and is a measure of the energy loss. That is, tan δ causes the vibration energy applied to the rubber composition to be dissipated as heat. Therefore, the smaller tan δ is, the less heat is dissipated. (i.e., internal heat generation is reduced and transmission efficiency is improved). In this case, the ta at the temperature at which the belt normally runs (for example, in the temperature range of 40 to 120°C) Focusing on nδ, the tan δ is adjusted to be low. To ensure transmission efficiency, the tan δ of the cured material at a frequency of 10 Hz must be 0.08 to 0. It can be selected from a range of about 17, for example, 0.09 to 0.165, preferably 0.09 to 0. 12, more preferably 0.09 to 0.11, and most preferably 0.09 to 0.10. The loss tangent (tan δ) value is a substitute value that indicates the internal heat generation property of a rubber composition. A small value is an indicator of a rubber composition with little internal heat generation and little energy loss (transmission loss). do.

[0085] In this specification and claims, the loss tangent (tan δ) is as described in the examples below. In the cured product in which the short fibers are aligned in a specific direction, the alignment direction of the short fibers ( The loss tangent is measured in the direction perpendicular to the grain direction (anti-grain direction).

[0086] [Method of manufacturing rubber composition] The method for producing the rubber composition of the present invention comprises mixing (or kneading) each component by a conventional method. However, in order to mix uniformly, it is preferable to heat and knead the ingredients. Furthermore, the production method of the present invention may be a production method in which the components are added at once and kneaded. The first kneading step is a step of kneading the main components other than the crosslinking component, and the second kneading step is a step of kneading the main components other than the crosslinking component. The product is kneaded in two stages, with a crosslinking component being added to the kneaded product and kneaded in the second kneading process. The manufacturing method is preferred.

[0087] In the manufacturing method using the two-stage kneading process, in the first kneading process, (B), a co-crosslinking agent, a vulcanization aid or vulcanization accelerator, and a sulfur-containing silyl peroxide (C), It is preferable to knead components other than the silane coupling agent (E). The coupling agent (E) is kneaded in the second kneading step, whereas the silane coupling agent (F) containing a double bond is kneaded in the third kneading step. By kneading the pulling agent (D) in the first kneading step, the dispersibility of the silica (C) is improved. The first kneading temperature in the first kneading step is higher than that in the second kneading step. For example, the temperature is 150° C. or higher (for example, about 150 to 200° C.).

[0088] In the second kneading step, the first kneaded product obtained in the first kneading step, the crosslinking component, It is preferable to knead the silane coupling agent (E) containing a sulfur atom. By kneading the coupling agent (E) in the second kneading step, the heat resistance of the rubber composition is improved. The second kneading temperature in the second kneading step is set to a lower temperature than the first kneading temperature. For example, the temperature is 120° C. or lower (for example, about 50 to 120° C.).

[0089] [Molded body] The cured product of the rubber composition of the present invention has both heat resistance and abrasion resistance, and can be used in various molded articles. Both properties are important for the transmission belt's transmission surface (contact surface with the pulley). It is preferable to use it as a rubber layer.

[0090] The power transmission belt may be a friction power transmission belt or a meshing power transmission belt. Examples of friction transmission belts include flat belts, wrapped V-belts, raw edge V-belts, Examples include V-belts such as raw edge cog V-belts and V-ribbed belts. Examples of the transmission belt include a toothed belt and a double-sided toothed belt. Among these, friction transmission belts are preferred because of the requirement for high heat resistance and abrasion resistance. V-ribbed belts used in auxiliary drive systems for car engines, and continuously variable transmissions for motorcycles Raw edge V-belts (including raw edge cogged V-belts) are more preferable. Due to the requirement for high durability, V is used in the auxiliary drive system of automobile engines. Ribbed belts are particularly preferred.

[0091] In friction transmission belts such as V-ribbed belts and raw edge V-belts, the rubber compound of the present invention is The composition forms a compression rubber layer (inner rubber layer) and / or a tension layer (back rubber layer) As a friction transmission belt in which the stretch layer is a back rubber layer, for example, Examples include V-ribbed belts that run in a rear drive layout that comes into contact with the rear wheels. Among them, a friction transmission belt in which at least a compression rubber layer is formed from the rubber composition of the present invention is preferred. stomach. EXAMPLES

[0092] The present invention will be described in more detail below with reference to examples. However, the raw materials used in the examples are not limited thereto. Details of the raw materials used in the examples are shown below.

[0093] [Raw materials] EPDM1: NORDEL (registered trademark) IP4640 manufactured by Dow Chemical Japan Co., Ltd. , Mooney viscosity (125°C) ≒ 40, ethylene content 55 mass%, diene content (ethylidene Norbornene content) 4.9% by mass EPDM2: Mitsui Chemicals "EPT 4045M", Mooney viscosity (125℃) ≒ 45, ethylene content 51% by mass, diene content 7.6% by mass EPDM3: NORDEL (registered trademark) IP3640 manufactured by Dow Chemical Japan Co., Ltd. , Mooney viscosity (125°C) ≒ 40, ethylene content 55% by mass, diene content 1.8% by mass Short fibers: Nylon 66 short fibers, average fiber diameter 27μm, average fiber length 3mm Silica 1: "Ultrasil VN3" manufactured by Evonik Industries AG, B ET specific surface area 180m 2 / g Silica 2: Ultrasil 9100GR manufactured by Evonik Industries AG ”, BET specific surface area 235m 2 / g Silane coupling agent 1-1: methacryloyl group-containing silane, manufactured by Shin-Etsu Chemical Co., Ltd. KBM-503, molecular weight 232, number of silicon atoms 1 Silane coupling agent 1-2: Vinyl-containing silane, Evonik Industries "Dynasylan VTEO" manufactured by AG, molecular weight 190, number of silicon atoms 1 Silane coupling agent 1-3: Vinyl group-containing silane, Evonik Industries A "Dynasylan 6498" manufactured by Company G, molecular weight 771, number of silicon atoms 6 Silane coupling agent 2-1: Disulfide group-containing silane, "CA BRUS-2, molecular weight 475, number of silicon atoms 2 Silane coupling agent 2-2: Tetrasulfide group-containing silane, manufactured by Osaka Soda Co., Ltd. CABRUS-4, molecular weight 539, number of silicon atoms 2 Zinc oxide: Seido Chemical Industry Co., Ltd., "Zinc oxide type 3" Stearic acid: NOF Corp., "Camellia Stearate" Paraffin oil: Paraffin-based process oil, "Diana (registered)" manufactured by Idemitsu Kosan Co., Ltd. Trademark)PW-380” Surfactant: "Newcol 2308-LY" manufactured by Nippon Nyukazai Co., Ltd. Antioxidant 1: Diphenylamine-based antioxidant, "Nocrack" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. "KCD" Antioxidant 2: Diphenylamine-based antioxidant, "Nocrack" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. KAD-F" Organic peroxide: NOF Corp.'s "Percumyl D" (dicumyl peroxide) Co-crosslinking agent: "Valnoc PM" manufactured by Ouchi Shinko Chemical Co., Ltd. Vulcanization accelerator DM: "Noccela (registered trademark) DM" manufactured by Ouchi Shinko Chemical Industry Co., Ltd. Carbon black HAF: "Seast 3" manufactured by Tokai Carbon Co., Ltd. Carbon black dispersion: Tokai Carbon Co., Ltd. "Aqua-Black 162" solid min19.2% by mass Core: 1,000 denier PET fiber, twisted 2x3, top twist factor 3.0, bottom twist factor 3.0 The twisted cord is made of multiple twisted yarns with a twist factor of 3.0 and a total denier of 6,000, and is then adhesively treated. The cord has a core diameter of 1.0 mm.

[0094] Examples 1 to 11, Reference Examples 1 to 7, and Comparative Examples 1 to 3 [Compressed rubber layer] The compression rubber layer that forms the belt transmission surface (contact surface with the pulley) is The rubber composition for the compressed rubber layer is kneaded in a Banbury mixer and then kneaded in a predetermined manner using a calendar roll. The sheet was rolled to a thickness of 100 mm. The details of the kneading method are as follows: The components other than the silane coupling agent 2-1 or 2-2, organic peroxide, and co-crosslinking agent are After the temperature reached 150°C, mixing was continued for 2 minutes, and the mixture was then discharged and allowed to cool. Next, in the second kneading step, the obtained kneaded product is mixed with a silane coupling agent 2-1 or 2-2. Organic peroxide and co-crosslinking agent (Comparative Examples 1 and 3 are organic peroxide and co-crosslinking agent only) The ingredients were added and kneaded, and when the temperature reached 100°C, the ingredients were immediately discharged.

[0095] In Reference Example 6, a silane coupling agent containing a sulfur atom was used. The same procedure as in Example 1 was repeated except that the mixing agent 2-1 was mixed in the first mixing step (150°C). The rubber composition was obtained by the above method.

[0096] In Reference Example 7, the same procedure was carried out except that the temperature of the first kneading step was 110°C. A rubber composition was obtained in the same manner as in Example 1.

[0097] [Table 1]

[0098] [Table 2]

[0099] [Adhesive rubber layer] The adhesive rubber layer sheet was prepared by mixing the adhesive rubber layer composition shown in Table 3 in a Banbury mixer. The mixture was kneaded and rolled to a predetermined thickness using a calendar roll.

[0100] [Table 3]

[0101] [Stretch layer] The cotton fabric used to form the stretch layer was untreated cotton fabric (cotton yarn 20s / 2, warp yarn 70 / 5cm, 70 wefts / 5cm plain weave) was mixed with carbon black dispersion and RFL liquid (lattice The mixture (black dye solution) shown in Table 4, which contains 100% ethylhexyl ether, 100% resorcinol, and 100% formalin, was then immersed in the mixture for 10 seconds. Cotton fabric that was immersed in water, tentered at a wide angle of 120°, and then heat-treated at 150°C for 4 minutes. Cloth was used.

[0102] [Table 4]

[0103] [Crosslinked rubber properties of the composition for the compressed rubber layer] The uncrosslinked rubber sheet for the compressed rubber layer was pressurized and heated (warmed) for 30 minutes using a press machine. A crosslinked rubber sheet was produced by subjecting the mixture to a temperature of 170°C and a surface pressure of 2.0 MPa.

[0104] 1) DIN wear volume A hollow drill with an inner diameter of 16.2 mm is used to drill a cross-linked rubber sheet with a diameter of 16.2 ± 0 mm from the thickness direction. A cylindrical test piece measuring 0.2 mm in diameter and 8 mm thick was cut out to prepare the test piece. JIS K6264 (2005), the amount of wear was measured using a DIN abrasion tester (rotating cylindrical abrasion tester). The polishing cloth was attached to the rotating drum by a polishing cloth holder, and the test method was to rotate the test piece. The test piece was subjected to a load of 10 N. The change in the amount of wear was measured, and the amount of wear (wear volume) was calculated from the specific gravity of the test piece that had been measured in advance. did.

[0105] 2) Measurement of loss tangent (tan δ) From the cross-linked rubber sheet, a rectangular cross-sectional shape (thickness 2.0 mm, width 4.0 mm, length A test piece of 40 mm was taken, with the anti-grain direction of rolling set as the length direction. Then, the chuck of the viscoelasticity measuring device ("VR-7121" manufactured by Ueshima Seisakusho Co., Ltd.) was The test piece was chucked and fixed with a chuck distance of 15 mm, and an initial strain (static strain) of 1.0% was applied. Frequency 10Hz, dynamic strain 0.2% (i.e., the initial strain of 1.0% is the center position or reference The specimen was heated at a rate of 1°C / min to 70°C while applying a ±0.2% strain in the longitudinal direction. The loss tangent (tan δ) was calculated.

[0106] 3) Measurement of tensile properties (elongation at break) JIS K 6251 (2010) "Vulcanized and thermoplastic rubber - Determination of tensile properties" According to the "Test on the Crosslinked Rubber Sheets", a dumbbell-shaped test piece No. 3 was cut from the crosslinked rubber sheet in the anti-grain direction and A tensile test was carried out at a temperature of 200°C and a tensile speed of 500 mm / min. The elongation (%) at the time when the test piece broke was calculated. The elongation was measured before and after heat aging.

[0107] In addition, accelerated aging tests were conducted according to JIS K 6257 (2010) at 150°C. After 720 hours of heat aging, the test pieces were also subjected to tension at room temperature at a tensile speed of 500 mm / min. A tensile test was performed, and the elongation (%) at the time when the test piece broke was calculated and used as the elongation after heat aging.

[0108] From the above results, the difference (decrease) in elongation rate before and after heat aging was compared, and the difference in elongation rate was small. It was determined that the more the composition, the less the degree of heat aging and the more excellent the heat resistance.

[0109] The tensile tester used was Shimadzu Corporation's Autograph AG-5000A. In the accelerated aging test, the A-2 forced circulation type heat aging tester (cross wind type) was used. there was.

[0110] [Manufacturing of V-ribbed belts] A cotton woven fabric is wrapped around the outer periphery of a cylindrical mold with a smooth surface to form a stretch layer. Then, an uncrosslinked adhesive rubber layer sheet was wrapped around the outer periphery of the cotton woven fabric. The twisted cord that will be the core is spun in a spiral shape at a specified interval around the outer periphery of the sheet. The uncrosslinked adhesive rubber layer sheet and the compressed rubber layer sheet are wound around the outer circumference of the uncrosslinked rubber layer. A molded body was formed. Then, the uncrosslinked molded body was covered with a vulcanization jacket. The mold with the crosslinked molded body attached is placed in a crosslinking device (a so-called vulcanizing can) and heated to a specified temperature. After crosslinking under pressure conditions (180℃, 0.9MPa), the product is removed from the mold and formed into a cylinder. The outer surface of the cross-linked sleeve was ground with a grinding wheel. After forming the desired V-rib portion, the bridging sleeve is cut in the belt longitudinal direction using a cutter blade. Cut to the specified width and use 5PK1100 V-ribbed belt (number of ribs: 5, circumference: 1100 mm, belt shape: K type, belt thickness: 4.3 mm, rib height: approx. 2 mm, rib pitch: 3 The cut belt was then turned over to the inside and outside to create a finished belt. As a result, a V-ribbed belt was obtained that had a compressed rubber layer having a V-rib portion on the inner peripheral side.

[0111] [Performance evaluation of V-ribbed belts] 1) Abrasion resistance test (6% slip test) Driving (Dr) pulley diameter 80 mm, driven (Dn) pulley diameter 80 mm, A running test machine was used with the layout shown in Figure 1, in which a tension (Ten) pulley of 1 mm was arranged. A V-ribbed belt, the weight of which had been measured in advance, was hung on each pulley of the testing machine, and tension was applied. The belt was wrapped around the drive pulley at a 90° angle, and the rotation speed of the drive pulley was measured at room temperature. The rotational speed is 3000 rpm, the torque of the driven pulley is 9.8 N m, and the belt slip rate is 6%. The belt tension was automatically adjusted as shown in the figure, and the machine was run for 24 hours. The weight of the belt was measured, and the reduction in the belt weight [(belt weight before running) - (belt weight after running) The ratio of the reduction in the belt weight to the weight of the belt before running [(Belt The wear rate was calculated as follows: (loss in belt weight) / (weight of belt before running) x 100 The progress was compared.

[0112] 2) Durability test (heat resistance and running life) A drive pulley 11 with an outer diameter of 120 mm, an idler pulley 12 with an outer diameter of 85 mm, and an outer diameter of 120 mm The layout shown in FIG. 2 is a pulley with a diameter of 45 mm, a driven pulley 13 with a diameter of 45 mm, and a tension pulley 14 with an outer diameter of 45 mm. A V-ribbed belt was hung on each pulley of the test machine, and an idle pulley was used. The belt wrap angle around the tension pulley is 120°, The angle was adjusted to 90° and the belt tension to 395N. The rotation speed of the drive pulley was 4900 rpm (rotation direction is the direction of the arrow in the figure), the load on the driven pulley is 8.8 kW, and the ambient temperature is 1 The temperature was 40°C and the maximum running time was 300 hours. The belt broke before reaching 300 hours. If a fault or abnormality occurs, the time is deemed to be the end of the lifespan and the operation is terminated. If no failure or abnormality occurs in the belt, it has a running life of 300 hours or more. The belts that had a running life of 300 hours or more in this test were deemed to be heat-resistant. It was judged to be a belt with excellent durability.

[0113] 3) Measurement of transmission loss (torque loss) It consists of a driving pulley (Dr) with a diameter of 55 mm and a driven pulley (Dn) with a diameter of 55 mm. A biaxial running test machine with the layout shown in Fig. 3 was used. A V-ribbed belt was hung on the test machine. The V-ribbed belt is given a specified initial tension of 500N per belt, and no driven pulley is required. The difference between the driving torque and the driven torque when the drive pulley is rotated at 2000 rpm under load. The torque loss calculated by this measurement is the same as that of the V-ribbed belt. In addition to the torque loss caused by the bearings of the test machine, the torque loss caused by the bearings of the test machine is also included. Therefore, the torque loss of the belt is considered to be virtually zero. The difference between the driving torque and the driven torque is calculated as the torque loop caused by the bearing. The torque loss was calculated by running the V-ribbed belt. (torque loss caused by both the belt and the bearings) to torque loss caused by the bearings (torque loss caused by the The torque loss due to the belt itself was calculated by subtracting the loss due to the bearing loss. The torque loss (bearing loss) is the torque loss when a metal belt is run with a specified initial tension. (For example, if a V-ribbed belt is run with an initial tension of 500N per belt, this initial tension (The torque loss when a metal belt is running at a constant speed is the bearing loss.)

[0114] When transmitting power, energy loss (transmission loss) occurs. The energy loss is, for example, an internal loss due to self-heating of the rubber composition constituting the belt, or a loss due to the temperature of the belt. The bending loss caused by the bending deformation of the drive shaft is usually The "torque loss" value, calculated as the difference between the driven torque value on the driven shaft, is the energy loss. It is used as an index of torque loss, and the smaller the torque loss, the better the transmission efficiency (the less the transmission loss). This is also used as an indicator of fuel efficiency in automobile engines. Based on the torque loss measurements, a comparison was made of transmission efficiency, which affects fuel economy.

[0115] The evaluation results of the Examples are shown in Table 5, and the evaluation results of the Reference Examples and Comparative Examples are shown in Table 6.

[0116] [Table 5]

[0117] [Table 6]

[0118] In Tables 5 and 6, the silane coupling agent is a double bond-containing silane coupling agent. Comparative Example 1, which used only a binder, is compared with the conventional level of durability in terms of heat resistance and abrasion resistance. The improvement in durability life (superiority or inferiority) was then compared based on this standard.

[0119] Two types of silane coupling agents (one containing a double bond and one containing a sulfur atom) are used in combination. The total amount (X1 + X2) and the ratio are parameters related to the amount of run coupling agent added. For (Y1 / Y2), both are within a specified range (X1+X2=0.0001~0.000 3, in Examples 1 to 11 in which Y1 / Y2=0.8 to 6) is satisfied, the transmission efficiency is The durability life has been improved while maintaining the torque loss. In particular, cracks caused by thermal degradation have been suppressed. The system had a significant effect.

[0120] In detail, in Examples 2 to 4 and 8, the above-mentioned silane coupling agent was used in comparison with the silane coupling agent in Example 1. Although the parameters were changed, the results in Examples 2 to 4 were almost the same as those in Example 1. Furthermore, a double bond-containing silane coupling agent and a sulfur atom-containing silane coupling agent The ratio (Y1 / Y2) is the same as in Example 1, and the sum of X1 and X2 in Example 1 In Example 8 (X1+X2=0.00018) the total value was increased to 0.00 026), the initial crosslinked rubber properties (elongation at break) were slightly lower than in Example 1. However, the durability (heat resistance) and transmission efficiency were equivalent to those of Example 1.

[0121] Even if a sulfur atom-containing silane coupling agent is added, the double bond-containing silane coupling agent In Comparative Example 2, in which no additive was added, the heat resistance of the crosslinked rubber was improved compared to Comparative Example 1. As a result, the torque loss increases due to the increase in internal heat generation, and the wear resistance decreases. After a long drive, the tire reached the end of its life due to slippage. This result also shows that two types of silane coupling agents ( It can be said that the combined use of a tertiary amine containing a double bond and a tertiary amine containing a sulfur atom is effective.

[0122] When two types of silane coupling agents (one containing a double bond and one containing a sulfur atom) are used together, In the above cases, in Reference Examples 1 to 3, the total amount (X1 + X2 ) and the ratio (Y1 / Y2) do not satisfy the predetermined range.

[0123] In Reference Example 1, in the ratio (Y1 / Y2), Y2 (a sulfur atom-containing silane coupling agent) Since the amount of additive added is too small, the effect of improving heat resistance is small compared to Comparative Example 1. In Example 2, in the ratio (Y1 / Y2), Y1 (the amount of double bond-containing silane coupling agent added) ) is too small, and thus the abrasion resistance is insufficient compared to Comparative Example 1. Although the durability and lifespan have improved, the torque loss has increased due to wear and the transmission efficiency cannot be maintained. Reference Example 3 is an example in which the total amount (X1 + X2) of two types of silane coupling agents is too small. The dispersibility of silica cannot be increased sufficiently, and the wear resistance is high due to poor dispersion. The torque loss also increased due to the increase in internal heat generation. The thermal degradation cracks could not be suppressed. This is an example where the total amount of coupling agent (X1 + X2) is too large, but the transmission efficiency is excellent. However, the initial crosslinked rubber properties (breaking elongation) were lower than those of Example 8, and the heat resistance was improved during durability testing. Deterioration caused early cracks.

[0124] Example 11 is an example in which the diene content is reduced compared to the EPDM of Example 1. In Example 11 (diene content 1.8% by mass), The physical properties of crosslinked rubber (elongation at break) were improved and heat resistance was also excellent, but internal heat generation increased. On the other hand, in Reference Example 4, two types of silane coupling agents ( Even when used in combination with other olefins (containing double bonds and sulfur atoms), the diene content is high. This is an example using EPDM of grade (7.6 mass%). The structure is the same as that of Example 1. In this case, the heat resistance of the crosslinked rubber is insufficient, so The effect of using two types of silane coupling agents (containing double bonds and sulfur atoms) in combination was obtained. The durability life was the shortest among the examples of the present invention and the comparative examples.

[0125] In Comparative Example 3, a sulfur atom-containing silane coupling agent was added to the composition of Comparative Example 1. This is an example of a case where the amount of antioxidant is increased. As in Example 1, where 1 was added, a significant effect was observed in suppressing cracks caused by thermal degradation. The durability life was improved compared to Comparative Example 1. However, compared to Comparative Example 1, internal heat generation increased and the torque The loss increased and the transmission efficiency could not be maintained. The method using a ring agent is advantageous in that it can improve heat resistance while maintaining transmission efficiency. It can be said that.

[0126] Examples 5 to 7 are examples in which the type of silane coupling agent used in Example 1 was changed. Both double bond-containing silane coupling agents and sulfur atom-containing silane coupling agents have molecular Even when other types having different amounts or numbers of silyl groups (number of silicon atoms) are used, the examples are As with Nos. 1 to 4, the transmission efficiency (torque loss) was maintained compared to Comparative Example 1, while the durability was improved. The results showed a significant effect on the above (especially in suppressing cracks caused by thermal degradation).

[0127] In Examples 9 and 10, the specific surface area and the blending ratio of the silica in Example 1 were changed. In Example 9, silica having a larger specific surface area than that of Example 1 was used. In Example 10, the same effect as in Examples 1 to 4 was obtained, and the wear resistance was further improved. The ratio of silane coupling agent to the total amount of X1 and X2 is kept constant (Y1 / Although the composition of Y2) is the same as that of Example 1, the amount of silica is increased. Although the wear resistance is improved by the reinforcement effect of the force, internal heat generation (torque loss) increases, and transmission efficiency is reduced. The rate has decreased.

[0128] Reference Examples 6 and 7 are examples in which the kneading conditions were changed from those of the manufacturing method of Example 1. In Example 6, the sulfur atom-containing silane coupling agent was kneaded under high temperature conditions. Unlike 1, the thermal degradation of the crosslinked rubber properties (elongation at break) was evident, and cracks due to thermal degradation were observed. The durability of the product was reduced by kneading the sulfur-containing silane coupling agent at high temperatures. As a result, the effect of the silane coupling agent containing sulfur atoms on heat resistance was not observed. Therefore, the kneading of the silane coupling agent containing sulfur atoms is performed at about 100°C. Low temperature conditions of 30°C are preferred.

[0129] In addition, in Reference Example 7, the temperature of the first kneading step is 110° C. (high temperature condition). Unlike Example 1, the wear resistance was significantly reduced during endurance driving. The silica also reached the end of its life due to slippage. It can be inferred that the wear resistance was reduced due to the lack of reinforcing effect of the silica. The first kneading step for achieving this is preferably carried out under high temperature conditions of 150° C. or higher. [Industrial Applicability]

[0130] The rubber composition of the present invention can be used as various molded articles, particularly as a transmission belt, e.g. Belts; Wrapped V-belts, Raw Edge V-belts, Raw Edge Cogged V-belts, V-ribbed Friction transmission belts such as belts, toothed belts, double-sided toothed belts and other meshing transmission belts It can be preferably used as.

Claims

1. A method for producing a rubber composition, comprising heating and kneading an ethylene-α-olefin elastomer (A), an organic peroxide (B), silica (C), a silane coupling agent containing an ethylenically unsaturated bond (D), and a silane coupling agent containing a sulfur atom (E), A production method comprising: a first kneading step of kneading components containing the ethylene-α-olefin elastomer (A), the silica (C), and the silane coupling agent (D) containing an ethylenically unsaturated bond at a kneading temperature of 150° C. or higher; and a second kneading step of kneading components containing the organic peroxide (B) and the silane coupling agent (E) containing a sulfur atom at a kneading temperature of 120° C. or lower, the rubber composition comprises the ethylene-α-olefin elastomer (A), the organic peroxide (B), the silica (C), the silane coupling agent containing an ethylenically unsaturated bond (D), and the silane coupling agent containing a sulfur atom (E); and The ethylene-α-olefin elastomer (A) has a diene content of 7% by mass or less, When the calculated value of X represented by the following formula (1) in the silane coupling agent (D) is X1, and the calculated value of X represented by the following formula (1) in the silane coupling agent (E) is X2, the total value of X1 and X2 is 0.0001 to 0.0003, The production method in which the ratio of Y1 to Y2 (Y1 / Y2) is 0.8 to 6, where Y1 is the calculated value of Y represented by the following formula (2) in the silane coupling agent (D) and Y2 is the calculated value of Y represented by the following formula (2) in the silane coupling agent (E). X=a×[b / (c×d)] (1) (In the formula, a represents the ratio of the silane coupling agent to 100 parts by mass of silica, b represents the number of silicon atoms in the silane coupling agent, c represents the BET specific surface area of ​​the silica, and d represents the molecular weight of the silane coupling agent.) Y=a×(b / d) (2) (wherein a, b and d are the same as above)

2. The method according to claim 1, wherein the proportion of the silica (C) is 25 to 120 parts by mass per 100 parts by mass of the ethylene-α-olefin elastomer (A).

3. 3. The process according to claim 1, wherein the proportion of the organic peroxide (B) is 1 to 8 parts by mass per 100 parts by mass of the ethylene-α-olefin elastomer (A).

4. The method according to any one of claims 1 to 3, wherein the rubber composition is used to form a transmission surface of a transmission belt.

Citation Information

Patent Citations

  • Silica-loaded rubber composition

    JP1998182885A

  • Frictional transmission belt

    JP2006194322A

  • Frictional transmission belt

    JP2006194357A

  • Power transmission belt and method of manufacturing power transmission belt

    JP2006275191A

  • Power transmission belt and its manufacturing method

    JP2008082538A