Copper alloy with excellent laser light absorption rate and its manufacturing method
By dispersing intermetallic compounds on copper alloys, the absorption rate is enhanced, addressing inefficiencies in laser processing, allowing for efficient and impurity-minimized laser processing.
Patent Information
- Application Number
- JP2020042181
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-11
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-03-11
AI Technical Summary
Copper and copper alloys have low laser light absorption rates in the near-infrared wavelength range used by fiber lasers, leading to inefficient processing due to high thermal conductivity and the formation of surface oxide films or plating which degrade thermal conductivity and introduce impurities.
Dispersing intermetallic compounds such as Cu1.96S, Cu2S, or Cu5Zr on the surface of copper alloys, which have a bandgap of about 1.2 eV, enhancing laser light absorption without the need for oxide films or plating, and heat-treating the alloys to precipitate these compounds.
The copper alloys exhibit a high absorption rate of 15-28% for fiber lasers, enabling efficient laser processing with improved thermal conductivity and reduced impurity influence, suitable for welding and cutting applications.
Smart Images

Figure 0007571377000002 
Figure 0007571377000003 
Figure 0007571377000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a copper alloy having excellent laser light absorption rate suitable for a process using a laser, and a method for producing the same. [Background technology]
[0002] In recent years, with the widespread use and improved performance of fiber lasers, technological developments have been made in processing processes such as welding and cutting using fiber lasers. Copper and copper alloys have problems in that melting using a laser is difficult or only efficient, due to the large energy diffusion caused by their high thermal conductivity and the low absorption rate of laser light in the near-infrared wavelength range used in fiber lasers.
[0003] For this reason, for example, as described in Patent Document 1 below, a method for improving the laser light absorption rate using a surface oxide coating or plating is known as a known technique. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 63-303693 Summary of the Invention [Problem to be solved by the invention]
[0005] However, the technique described in Patent Document 1 has a problem in that the amount of oxygen in the shaped product increases due to the formation of an oxide film, which in turn reduces the thermal conductivity. Furthermore, with regard to the laser absorption rate due to plating treatment, there is a problem in that the properties such as the thermal conductivity of the copper base material are reduced due to alloying with the plating components during melting.
[0006] The present invention has been devised in view of the above problems, and an object of the present invention is to provide a copper alloy which is suitable for laser processing and has an improved laser light absorption rate, and a method for producing the same. [Means for solving the problem]
[0007] In order to achieve the above-mentioned objective, it is considered effective to precipitate on the surface an intermetallic compound having a band gap of about 1.2 eV, which corresponds to 1064 nm, the central wavelength of a fiber laser.
[0008] Therefore, the inventors have conducted various studies and found that Cu 1.96 S, Cu 2 Either or both of S or Cu 5 It was discovered that if an intermetallic compound made of Zr is dispersed on the surface of a copper alloy, it is possible to provide a copper alloy with high laser light absorption. 。 Cu 1.96 S, Cu 2 S, Cu 5 The intermetallic compound represented by Zr is thought to have a band gap of about 1.2 eV, which is smaller than the band gap of pure copper alone. Therefore, if these intermetallic compounds are dispersed on the surface of a copper alloy, a copper alloy with high laser light absorption rate can be provided, and a copper alloy suitable for laser processing can be provided.
[0009] ( 1 A copper alloy having excellent laser light absorptivity according to one embodiment of the present invention contains 0.03 mass% or more and 1.0 mass% or less of S, with the remainder being unavoidable impurities and Cu. 1.96 S, Cu 2the intermetallic compounds dispersed in a cross section of the copper alloy have an area fraction of 4.3% or more and 15.6% or less, the optical absorptance of a fiber laser having a central wavelength of 1064 nm is 18% or more and 28% or less, and the unavoidable impurities have a total concentration of unavoidable impurities excluding gas components C, N, and O in a range of 5 ppm by mass or more and 50 ppm by mass or less, and the gas components C, N, and O have a total concentration of 10 ppm by mass or more and 10,000 ppm by mass or less. ( 2 A copper alloy having excellent laser light absorption rate according to one embodiment of the present invention contains 0.03 mass% or more and 0.20 mass% or less of Zr, the remainder being unavoidable impurities and Cu, 5 The copper alloy has a structure in which a plurality of intermetallic compounds made of Zr are dispersed, the plurality of intermetallic compounds dispersed in a cross section of the copper alloy are dispersed at an area fraction of 3.0% or more and 5.5% or less, the optical absorptance of a fiber laser having a central wavelength of 1064 nm is 15% or more and 18% or less, and the unavoidable impurities have a total concentration of unavoidable impurities excluding gas components C, N, and O in a range of 5 ppm by mass or more and 50 ppm by mass or less, and the gas components C, N, and O have a total concentration of 10 ppm by mass or more and 10,000 ppm by mass or less.
[0010] ( 3 A method for producing a copper alloy having excellent laser light absorption rate according to one embodiment of the present invention comprises the steps of: forming a copper alloy containing 0.01 mass% or more and 1.0 mass% or less of S or Zr, with the remainder being unavoidable impurities and Cu; 1.96 S, Cu 2 Either or both of S or Cu 5 A method for producing a copper alloy having excellent laser light absorption rate, in which a plurality of intermetallic compounds made of Zr are dispersed, and the plurality of intermetallic compounds dispersed in a cross section of the copper alloy are dispersed at an area fraction of 3.0% or more and 16% or less, is characterized in that a copper alloy obtained by solidifying a molten copper alloy containing S or Zr by vacuum casting is subjected to a heat treatment under conditions of 300°C or more and 800°C or less.
[0011] (4 A method for producing a copper alloy having excellent laser light absorption rate according to one embodiment of the present invention comprises the steps of: 1.96 S, Cu 2 a copper alloy having a structure in which a plurality of intermetallic compounds consisting of either one or both of S and S are dispersed, the plurality of intermetallic compounds dispersed in a cross section of the copper alloy being dispersed at an area fraction of 4.3% or more and 15.6% or less, the optical absorptance of a fiber laser having a central wavelength of 1064 nm being 18% or more and 28% or less, and the unavoidable impurities, excluding the gas components C, N, and O, have a total concentration of unavoidable impurities in the range of 5 ppm by mass or more and 50 ppm by mass or less, and the gas components C, N, and O have a total concentration of 10 ppm by mass or more and 10,000 ppm by mass or less, the copper alloy being characterized in that the copper alloy obtained by solidifying a molten copper alloy containing S in the above ranges by vacuum casting is subjected to a heat treatment under conditions of 400°C or more and 800°C or less. ( 5 A method for producing a copper alloy having excellent laser light absorption rate according to one embodiment of the present invention comprises the steps of: 5 A method for producing a copper alloy having excellent laser light absorptance, the copper alloy having a structure in which a plurality of intermetallic compounds made of Zr are dispersed, the plurality of intermetallic compounds dispersed in a cross section of the copper alloy being dispersed at an area fraction of 3.0% or more and 5.5% or less, the light absorptance of a fiber laser having a central wavelength of 1064 nm being 15% or more and 18% or less, and the inevitable impurities, excluding the gas components C, N, and O, have a total concentration of unavoidable impurities in the range of 5 ppm by mass or more and 50 ppm by mass or less, and the gas components C, N, and O have a total concentration of 10 ppm by mass or more and 10,000 ppm by mass or less, the method being characterized in that a copper alloy obtained by solidifying a molten copper alloy containing Zr in the above range by vacuum casting is subjected to a heat treatment under conditions of 400°C or more and 700°C or less. Effect of the Invention
[0012] According to a copper alloy according to one embodiment of the present invention, Contains a specific amount of SMultiple particles are distributed throughout the cross section of the copper alloy. Cu 1.96 S and Cu 2 S of At least one The intermetallic compound is Specific Dispersed by surface fraction, unavoidable impurities By keeping the C, N, O and other components low, Since it has excellent absorption rate of laser light at 1064 nm, which is the central wavelength of fiber lasers, it can be melted using a fiber laser, making it suitable for use as a copper alloy for laser processing. According to one embodiment of the copper alloy of the present invention, a plurality of Cu particles are dispersed in a cross section of the copper alloy containing a specific amount of Zr. 5 The intermetallic compound made of Zr is dispersed at a specific surface fraction, and the inevitable impurities of C, N, O, and other components are kept low, resulting in excellent absorption of laser light at 1064 nm, the central wavelength of fiber lasers. This makes it possible to melt the material using a fiber laser, making it suitable for use as a copper alloy for laser processing. In addition, the copper alloy according to one embodiment of the present invention does not require an oxide film or plating on the surface, and therefore can minimize the influence of impurities such as oxygen, compared to conventional copper alloys that required an oxide film or plating. Therefore, by using the copper alloy according to one embodiment of the present invention, it is possible to manufacture a copper alloy member that does not increase the amount of oxygen in the copper alloy after processing and does not cause a decrease in thermal conductivity. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 is a diagram showing an example of joining of copper alloy sheets according to the first embodiment, where (A) is a plan view and (B) is a side view. [Diagram 2] FIG. 2 is an enlarged photograph showing the metal structure of the copper alloy produced in Example 1 after heat treatment. [Diagram 3] FIG. 3 shows the results of component mapping analysis of the metal structure shown in FIG. [Figure 4] FIG. 4 is an enlarged photograph showing the metal structure of the copper alloy produced in Comparative Example 1 before heat treatment. [Diagram 5] FIG. 5 is a graph showing X-ray diffraction patterns of the copper alloy produced in Example 1 before and after the heat treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The present invention will be described in detail below, but the present invention is not limited to the embodiments described below. The composition of the copper alloy according to the present embodiment is not particularly limited, but a copper alloy containing one or both of S and Zr in an amount of 0.01 mass% to 1.0 mass%, with the balance being unavoidable impurities and Cu, can be mainly used. 1.96 S, Cu 2 Either or both of S or Cu 5 The copper alloy must contain a plurality of intermetallic compounds represented by the composition formula of Zr. The copper alloy may contain inevitable impurity elements other than gas components, which will be described below. If the S or Zr content is less than 0.01 mass%, the amount of the desired intermetallic compound precipitated is small or no precipitation of the intermetallic compound is observed, and the light absorptance in the 1064 nm band is not improved. If the S or Zr content exceeds 1.0 mass%, the light absorptance is not significantly improved, but it is a factor in increasing costs, which is undesirable for industrial use.
[0015] (Inevitable impurity elements) Regarding the unavoidable impurities, the electrical conductivity and thermal conductivity characteristics are improved by lowering their concentrations. On the other hand, if an attempt is made to reduce the concentration of the unavoidable impurities more than necessary, the manufacturing process becomes complicated and the manufacturing cost increases significantly. Therefore, in this embodiment, the concentration of the unavoidable impurities excluding the gas components (C, N, O) is set to a range of 5 mass ppm to 50 mass ppm in total, and the concentration of the gas components (C, N, O) is set to a range of 10 mass ppm to 10,000 mass ppm in total. In order to keep the concentration of unavoidable impurities excluding gas components (C, N, O) within a range of 5 mass ppm or more and 50 mass ppm or less, and the concentration of gas components (C, N, O) within a range of 10 mass ppm or more and 10,000 mass ppm or less, high purity copper with a purity of 99 to 99.9999 mass% or oxygen-free copper (C10100, C10200) can be used as the raw material.
[0016] In order to reliably suppress an increase in manufacturing costs, the lower limit of the inevitable impurities other than the gas components (C, N, O) is preferably 10 mass ppm or more, and more preferably 15 mass ppm or more. On the other hand, in order to reliably improve the electrical conductivity and thermal conductivity, the upper limit of the inevitable impurities other than the gas components (C, N, O) is preferably 45 mass ppm or less, and more preferably 40 mass ppm or less.
[0017] Here, the inevitable impurities excluding the gas components (C, N, O) in this embodiment are one or more of Fe, Ni, As, Ag, Sn, Sb, Pb, Bi, P, Li, Be, F, Na, Mg, Al, Si, Cl, K, Sc, Ti, V, Cr, Mn, Nb, Co, Zn, Ga, Ge, Br, Rb, Sr, Y, Mo, Ru, Pd, Cd, In, I, Cs, Ba, rare earth elements, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg, Tl, Th, and U.
[0018] "Intermetallic compounds" The intermetallic compound is Cu 1.96 S, Cu 2 Either or both of S or Cu 5 The copper alloy is made of Zr and is formed by a vacuum casting method described later, and the copper alloy is heat-treated at 300 to 800° C. The heat treatment temperature is more preferably 300 to 600° C. In copper alloys produced by quenching from a molten metal using the vacuum casting method described below, S and Zr are contained in a supersaturated solid solution in the copper alloy base. By subjecting this copper alloy to heat treatment, multiple intermetallic compounds of Cu and S or Zr can be precipitated, and a copper alloy with excellent laser light absorption can be obtained. Cu 1.96 S, Cu 2 Either or both of S or Cu 5The intermetallic compound represented by Zr is thought to have a band gap of about 1.2 eV, which corresponds to 1064 nm, the central wavelength of the fiber laser. Therefore, compared to the band gap of Cu, which is usually considered to be about 2 eV, the intermetallic compound absorbs energy due to the precipitation and dispersion of the above-mentioned intermetallic compound, which can transition at a lower energy, and it is thought that the absorption rate of the copper alloy for the laser light of the fiber laser is improved.
[0019] FIG. 1(A) is a plan view showing, as an example, a joined body 3 formed by laser welding two rectangular plate-shaped plate materials 1 and 2 made of the above-mentioned copper alloy, and FIG. 1(B) is a side view of the joined body 3. In this example, the joined body 3 is formed by overlapping the longitudinal ends of the plate materials 1 and 2 over a predetermined width to form an overlapping portion 5. A fiber laser is irradiated over a predetermined length along the width direction of the plate materials 1 and 2 at the center of this overlapping portion 5 to heat and melt the irradiated portion, forming a welded portion 6. The plate materials 1 and 2 are joined by this welded portion 6 to form the joined body 3.
[0020] The plate materials 1 and 2 shown in Figures 1(A) and 1(B) are made of the above-mentioned copper alloy, and because they have a high fiber laser absorption rate, the parts irradiated with the fiber laser can be easily heated and melted. Therefore, efficient welding is possible when creating a joint 3 by laser welding. As described above, the above-mentioned copper alloy has excellent laser weldability. Therefore, not only the plate materials 1 and 2, but also members of various shapes to be laser-welded can be formed from the above-mentioned copper alloy to provide members with excellent laser weldability.
[0021] "Method of manufacturing copper alloys" As an example of a method for producing a copper alloy according to the present embodiment, high purity copper having a purity of 99.99% by mass or more and less than 99.9999% by mass and a Cu-S or Cu-Zr master alloy are used as raw materials in a vacuum, and are adjusted to have a composition shown in Table 1 below. For example, the copper alloy is adjusted to contain 0.01% by mass or more and 1.0% by mass or less of S or Zr, with the balance being unavoidable impurities and Cu. In addition, for S or Zr, a master alloy of each element can be prepared from S or Zr with a purity of 99% by mass or more and pure copper with a purity of 99.9% by mass, and the master alloy can be used for adjustment. The copper alloy can be obtained by solidifying the molten copper alloy obtained by melting in a crucible.
[0022] In this embodiment, an example using vacuum casting has been described, but the copper alloy may be produced by other methods such as sand casting, precision casting, and continuous casting.
[0023] The copper alloy obtained by the above-mentioned method is subjected to shaping processing such as rolling and cutting as necessary, and then heat treatment is performed using an atmospheric heating furnace under temperature conditions of 300° C. or more and 800° C. or less, more preferably 400° C. or more and 600° C. or less, for about 10 minutes to 120 minutes, for example, for about 60 minutes, followed by cooling. This heat treatment causes Cu to be added to the metal structure of the copper alloy. 1.96 S, Cu 2 Either or both of S or Cu 5 It is possible to precipitate intermetallic compounds made of Zr. These intermetallic compounds are fine particulate precipitates with a grain size of about 1 μm or less, and multiple precipitates are randomly precipitated within the crystal grains or at the grain boundaries of the copper alloy.
[0024] In the case of the copper alloy mentioned above, the laser light absorption rate for a fiber laser with a central wavelength of 1064 nm is high, so the copper alloy can be efficiently heated by irradiating it with fiber laser light to perform welding or cutting. Therefore, when additive manufacturing is performed using the above-mentioned copper alloy, it is possible to manufacture an additive manufacturing object that has high density, few pores, and high hardness. In addition, it is possible to provide a member with excellent laser weldability by using the above-mentioned copper alloy. EXAMPLES
[0025] A required amount of Cu-S alloy or Cu-Zr alloy was added to high purity copper with a purity of (99.999) mass%, and the mixture was put into a vacuum melting furnace to produce a molten copper alloy, which was then solidified to obtain an ingot of the copper alloy. The obtained copper alloy ingot was processed into a plate shape of 50 mm x 200 mm x 0.5 mm thick. Then, each copper alloy plate was heat treated under the heat treatment conditions (heating temperature: °C, heating time: hours) shown in Table 1 to obtain a copper alloy plate in which an intermetallic compound was precipitated.
[0026] The results of measuring the S or Zr content, the identity of the precipitate phase, the dispersion state of the precipitate phase, and the absorptance to light with a wavelength of 1064 nm for the obtained copper alloy sheets are shown in Table 1. The S content, the identity of the precipitate phase, the dispersion state of the precipitate phase, and the absorptance to light with a wavelength of 1064 nm were measured by the methods described below.
[0027] "S content" The S concentration in the copper alloy sheets was measured using a HORIBA (HORIBA, Ltd.) EMIA-810W (tubular furnace combustion-infrared absorption method). "Zr content" The Zr concentration in the copper alloy sheets was measured using an inductively coupled plasma emission spectrometer ICAP-88 manufactured by Nippon Jarrell Ash. "Identification of precipitates" The precipitates in the copper alloy sheets of each example were identified by measuring the diffraction patterns using an X-ray diffractometer, and it was confirmed that Cu-S or Cu-Zr intermetallic compounds were formed.
[0028] "Dispersion state of precipitates" The cross section of the copper alloy sheet was photographed by SEM, and the precipitates were identified in the cross section photograph using the image analysis software WinROOF, and the area ratio of the precipitates was calculated. At that time, SEM-EDS was used to confirm that the precipitates photographed were phases containing S or Zr, and an analysis was performed. "Absorptivity for 1064 nm wavelength light" The light absorptance of the copper alloy sheet of each example was measured using a "Ultraviolet-Visible-Near-Infrared Spectrophotometer U-4100" manufactured by Hitachi High-Tech Science Corporation. The total reflectance at 1064 nm, which is the central wavelength of the fiber laser, was measured, and the light absorptance (%) was calculated from the relational equation: light absorptance = (1 - total reflectance). The above results are shown in Table 1.
[0029] Next, the weldability was evaluated using heat-treated copper alloy sheets (Examples 1 to 5 and Comparative Examples 3 and 4) and non-heat-treated copper alloy sheets (Comparative Examples 1 and 2). To evaluate weldability, two copper alloy plates (copper alloy sheets) measuring 50 mm wide x 200 mm long x 0.5 mm thick were overlapped and fixed in an area of 50 mm x 50 mm, and then overlap welding of 0.5 mm wide x 30 mm long was performed using a 400 W fiber laser. The obtained sheet joint was evaluated for the presence or absence of peeling when a tensile load of 10 N was applied. The above measurement results are summarized in Table 1 below.
[0030] [Table 1]
[0031] As shown in Table 1, in Examples 1 to 5, Cu was deposited on the surface of the copper alloy containing S or Zr. 1.96 S, Cu 2 Either or both of S or Cu 5 Since the material has a structure in which multiple intermetallic compounds made of Zr are dispersed, it is possible to obtain high light absorption in the near infrared region, and no peeling is observed after laser welding. As a result of analysis from cross-sectional observation, it was confirmed that intermetallic compounds were dispersed in the copper alloys of Examples 1 to 5 at a cross-sectional area ratio of 3.0% or more (3.0 to 15.6%). In Table 1, ND means Not Detected.
[0032] The copper alloys of Examples 1 to 5 contain 0.01 mass% or more and 1.0 mass% or less of S or Zr, with the remainder being unavoidable impurities and Cu. 1.96 S, Cu 2 Either or both of S or Cu 5 This is a copper alloy having a structure in which multiple intermetallic compounds made of Zr are dispersed. It is also found that the intermetallic compounds are dispersed in these copper alloys at an area fraction of 3.0% or more and 16% or less. Furthermore, these copper alloys showed excellent light absorptance of 15 to 26% at a central wavelength of 1064 nm. Therefore, the sheet joints of Examples 1 to 7 were sufficiently laser welded and did not peel off.
[0033] FIG. 2 shows an enlarged photograph of the metal structure of the copper alloy sheet of Example 2 (heat treated at 500° C. for 1 hour). As shown in Figure 2, it was confirmed that multiple particulate intermetallic compounds with a diameter of 1 μm or less were precipitated within the crystal grains or at the crystal grain boundaries. The scale shown in the lower right of Figure 2 is 5 μm.
[0034] In contrast, the copper alloys of Comparative Examples 1 and 2 contain S or Zr, but are not heat-treated, and therefore no precipitation of intermetallic compounds is observed. As a result, the copper alloys of Comparative Examples 1 and 2 have low light absorptance and insufficient weldability. In the copper alloys of Comparative Examples 3 and 4, the concentration of S or Zr contained in the copper alloy is low, at 0.01% or less, and therefore no precipitation of intermetallic compounds is observed even when heat treatment is performed. For this reason, the light absorption rate is similarly low and the weldability is also insufficient.
[0035] FIG. 4 is a microstructure photograph showing the metal structure of the copper alloy before heat treatment, in contrast to the metal structure of the copper alloy shown in FIG. As is clear from comparing Figures 2 and 4, multiple fine intermetallic compounds are found to have precipitated in the heat-treated sample. Furthermore, when elemental analysis was performed at the same position at the same magnification as in the photograph shown in Figure 2, it was found that the S concentration in the precipitated area was extremely high. Figure 3 shows the results of elemental analysis of the region where multiple intermetallic compounds are precipitated in the metal structure of the copper alloy shown in Figure 2. The light-colored areas in the analysis results of S shown in the right side of Figure 3 correspond to the dark-colored granular areas in the metal structure shown in the left side of Figure 3. The lightly colored areas in the right-hand image of Figure 3 indicate areas with a high concentration of S. For this reason, the circular areas in Figure 2 can be assumed to be Cu-S intermetallic compounds.
[0036] Next, the diffraction pattern of the sample of Example 1 shown in Table 1 was determined by an X-ray diffractometer, and the result is shown in FIG. In the diffraction pattern shown in FIG. 5, the sharp large peaks present at around 44 degrees and 50 degrees are patterns derived from copper. In addition, the small peaks around 27 degrees, 33 degrees, 39 degrees, and 45 degrees in Figure 5 are Cu 1.96 This peak is due to S. Therefore, the precipitates on the surface of the copper alloy are Cu 1.96 It was found to be an intermetallic compound with the composition S. In addition, the diffraction pattern of the copper alloy of Example 2 was obtained by an X-ray diffraction device in the same manner. 2 A peak due to an intermetallic compound with the composition Cu was confirmed. 2 The intermetallic compound having a composition of S has peaks in its diffraction pattern at approximately 25 degrees, 27 degrees, 29 degrees, 31 degrees, 33 degrees, 35 degrees, 37 degrees, 38 degrees, 41 degrees, 47 degrees, and 49 degrees. In addition, the diffraction pattern of the copper alloy of Example 6 was obtained by an X-ray diffractometer. 5 A peak due to an intermetallic compound with a composition of Zr was confirmed. Cu 5 The intermetallic compound having a composition of Zr has peaks at approximately 36.9 degrees and approximately 46.7 degrees in its diffraction pattern.
[0037] From the above comparison, Cu is the most suitable for laser processing. 1.96 S, Cu 2 Either or both of S or Cu 5 It was found that a copper alloy having a structure in which multiple intermetallic compounds made of Zr are dispersed can obtain high light absorption and therefore good weldability. [Explanation of symbols]
[0038] 1, 2...plate material, 3...joint, 5...lapped part, 6...welded part.
Claims
1. A copper alloy containing 0.03 mass% or more and 1.0 mass% or less of S and the remainder being inevitable impurities and Cu, 1.96 S, Cu 2 The alloy has a structure in which a plurality of intermetallic compounds composed of either or both of S are dispersed, a plurality of intermetallic compounds dispersed in a cross section of the copper alloy are dispersed at an area fraction of 4.3% or more and 15.6% or less, and a light absorptance of a fiber laser having a central wavelength of 1064 nm is 18% or more and 28% or less; The copper alloy having excellent laser light absorptivity is characterized in that, in the unavoidable impurities, the concentration of unavoidable impurities excluding gas components C, N, and O is in the range of 5 ppm by mass or more and 50 ppm by mass or less in total, and the concentrations of the gas components C, N, and O are in the range of 10 ppm by mass or more and 10,000 ppm by mass or less in total.
2. A copper alloy containing 0.03 mass% or more and 0.20 mass% or less of Zr, the balance being unavoidable impurities and Cu, 5 The alloy has a structure in which a plurality of intermetallic compounds made of Zr are dispersed, a plurality of intermetallic compounds dispersed in a cross section of the copper alloy are dispersed at an area fraction of 3.0% or more and 5.5% or less, and a light absorptance of a fiber laser having a central wavelength of 1064 nm is 15% or more and 18% or less; The copper alloy having excellent laser light absorptivity is characterized in that, in the unavoidable impurities, the concentration of unavoidable impurities excluding gas components C, N, and O is in the range of 5 ppm by mass or more and 50 ppm by mass or less in total, and the concentrations of the gas components C, N, and O are in the range of 10 ppm by mass or more and 10,000 ppm by mass or less in total.
3. A copper alloy containing 0.01 mass % or more and 1.0 mass % or less of S or Zr, with the balance being inevitable impurities and Cu, 1.96 S, Cu 2 Either or both of S or Cu 5 A plurality of intermetallic compounds made of Zr are dispersed, The method for producing a copper alloy having excellent laser light absorptivity, the copper alloy having a structure in which a plurality of intermetallic compounds dispersed in a cross section of the copper alloy are dispersed at an area fraction of 3.0% or more and 16% or less, is characterized in that a copper alloy obtained by solidifying a molten copper alloy containing S or Zr by vacuum casting is subjected to a heat treatment under conditions of 300°C or more and 800°C or less.
4. A copper alloy containing 0.03 mass% or more and 1.0 mass% or less of S and the remainder being inevitable impurities and Cu, 1.96 S, Cu 2 a copper alloy having a structure in which a plurality of intermetallic compounds consisting of either one or both of S and S are dispersed, the plurality of intermetallic compounds dispersed in a cross section of the copper alloy being dispersed at an area fraction of 4.3% or more and 15.6% or less, the optical absorptivity of a fiber laser having a central wavelength of 1064 nm being 18% or more and 28% or less, and the inevitable impurities having a total concentration of inevitable impurities excluding gas components C, N, and O being 5 ppm by mass or more and 50 ppm by mass or less, and a total concentration of gas components C, N, and O being 10 ppm by mass or more and 10,000 ppm by mass or less, the copper alloy having an excellent laser light absorptivity being characterized in that a copper alloy obtained by solidifying a molten copper alloy containing S in the above ranges by vacuum casting is subjected to a heat treatment under conditions of 400° C. or more and 800° C. or less.
5. A copper alloy containing 0.03 mass% or more and 0.20 mass% or less of Zr, the balance being unavoidable impurities and Cu, 5A method for producing a copper alloy having excellent laser light absorptance, the method comprising the steps of: solidifying a molten copper alloy containing Zr within the above range by vacuum casting; heat treating the copper alloy obtained by solidifying a molten copper alloy containing Zr within the above range at a temperature of 400° C. or higher and 700° C. or lower; and wherein the copper alloy has a structure in which a plurality of intermetallic compounds made of Zr are dispersed in a cross section of the copper alloy at an area fraction of 3.0% or higher and 5.5% or lower; and the optical absorptance of a fiber laser having a central wavelength of 1064 nm is 15% or higher and 18% or lower; and the unavoidable impurities have a total concentration of unavoidable impurities excluding gas components C, N, and O in a range of 5 ppm by mass or higher and 50 ppm by mass or lower, and a total concentration of gas components C, N, and O in a range of 10 ppm by mass or higher and 10,000 ppm by mass or lower.
Citation Information
Patent Citations
High energy radiation working method
JP1988303693A
Copper alloy material, manufacturing method of copper alloy material, and cage type rotor
JP2018178189A
Metal powder and method for producing the same, and lamination-molded article and method for producing the same