Tape reels and tape cartridges
The tape reel design with a specific flange configuration and manufacturing apparatus addresses deformation issues, stabilizing tape reels in high-temperature, high-humidity conditions and improving recording and playback stability.
Patent Information
- Application Number
- JP2021043930
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-17
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-03-17
AI Technical Summary
Existing tape reel designs suffer from deformation issues due to increased winding tightness and storage in high-temperature, high-humidity environments, leading to instability in recording and playback characteristics of magnetic tapes.
A tape reel design featuring a cylindrical reel hub with a first and second flange, where the outer peripheral surface includes a first region with increasing diameter and a second region forming a convex ridgeline, along with a manufacturing apparatus using specific molds to shape the reel hub.
The design stabilizes the magnetic tape winding, reduces deformation, and maintains consistent tape edge contact with flanges, enhancing recording and playback performance.
Smart Images

Figure 0007571638000002 
Figure 0007571638000003 
Figure 0007571638000004
Abstract
Description
[Technical field]
[0001] The present technology relates to a tape reel having a cylindrical reel hub, a tape cartridge including the same, and a tape reel manufacturing apparatus. [Background technology]
[0002] Among magnetic tape cartridges used as external recording media for computers and the like, there is known a type in which a single tape reel around which a magnetic tape is wound is rotatably housed within a cartridge case. The tape reel has a cylindrical reel hub around which the magnetic tape is wound, and an upper flange and a lower flange disposed on both ends of the reel hub. A typical tape reel has a lower flange formed integrally with the reel hub, and an upper flange fixed to the upper end of the reel hub by ultrasonic bonding or the like.
[0003] In recent years, as the recording capacity of tape cartridges has increased, magnetic tapes have become thinner and longer, so the winding pressure (winding pressure) of the magnetic tape applied to the reel hub has been increasing. Furthermore, the winding pressure applied to the reel hub has been further increased due to the effects of long-term storage of tape cartridges in high-temperature and high-humidity environments, which has resulted in an increasing amount of deformation of the reel hub.
[0004] For example, in a reel structure in which the reel hub is molded integrally with the lower flange, the upper end of the reel hub fixed to the upper flange is deformed so as to fall inward, increasing the difference in outer diameter between both ends of the reel hub. As a result, the lower edge of the magnetic tape facing the lower flange is deformed so as to become longer than the upper edge of the magnetic tape facing the upper flange, which may cause the recording and playback characteristics of the magnetic tape to deteriorate.
[0005] To solve such problems, for example, Patent Document 1 listed below discloses a tape reel that includes a hub around which the recording tape is wound and flanges provided on both ends of the hub, with the hub forming a large diameter portion whose diameter is larger than the diameter of both ends.
[0006] Furthermore, Patent Document 2 listed below discloses a tape reel in which a cylindrical reinforcing ring is attached to a cylindrically formed hub, and the outer circumferential surface of the hub is tapered so that the outer diameter of the hub increases from its lower end to its upper end. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2008-243294 A [Patent Document 2] JP 2009-48692 A Summary of the Invention [Problem to be solved by the invention]
[0008] However, in the structure described in Patent Document 1, deformation of the central region of the tape wound around the large diameter portion of the hub outer circumferential surface can be a problem. For example, in a high temperature and high humidity storage environment, the shrinkage stress applied to the tape increases, so that the central region of the magnetic tape wound around the large diameter portion of the hub outer circumferential surface may deform excessively compared to the tape edge portions, which may adversely affect stable recording and playback characteristics.
[0009] Furthermore, in the structure described in Patent Document 2, the tapered shape of the hub outer peripheral surface is formed so that the inclination angle with respect to the lower flange gradually increases from the bottom end to the top end of the hub. This poses manufacturing disadvantages when the reel hub is molded integrally with the lower flange, such as making it difficult to ensure the draft angle of the mold that molds the outer peripheral surface of the reel hub.
[0010] In view of the above circumstances, an object of the present technology is to provide a tape reel that can suppress deformation of the reel hub caused by tight winding of the magnetic tape or the storage environment, a tape cartridge including the same, and a tape reel manufacturing device. [Means for solving the problem]
[0011] A tape reel according to one embodiment of the present technology includes a first flange, a second flange, and a cylindrical reel hub. The reel hub has a first end formed integrally with the first flange, a second end to which the second flange is joined, and an outer circumferential surface around which a magnetic tape is wound. The outer circumferential surface of the reel hub has a first outer circumferential region and a second outer circumferential region. The first outer circumferential region expands in diameter from the first end toward the second end. The second outer circumferential region expands in diameter from the first outer circumferential region to the second end, and forms a ridge portion on the boundary with the first outer circumferential region that is convex radially outwardly of the hub portion.
[0012] A tape cartridge according to one embodiment of the present technology includes a tape reel having a first flange, a second flange, and a cylindrical reel hub having a first end connected to the first flange, a second end connected to the second flange, and an outer circumferential surface around which a magnetic tape is wound. The outer circumferential surface of the reel hub is a first outer circumferential region that expands in diameter from the first end toward the second end; The reel hub has a second outer circumferential region that expands in diameter from the first outer circumferential region to the second end and forms a ridge portion that is convex radially outward of the reel hub on the boundary with the first outer circumferential region.
[0013] A tape reel manufacturing apparatus according to one embodiment of the present technology includes a first mold for forming an outer circumferential surface of the reel hub, and a second mold for forming an inner circumferential surface of the reel hub. The first mold has a first molding surface composed of a tapered surface that forms the first outer circumferential region, and a second molding surface composed of a cylindrical surface that forms the second outer circumferential region. [Brief description of the drawings]
[0014] [Figure 1] 1A and 1B are overall perspective views of a tape cartridge 1 according to an embodiment of the present technology, where FIG. 1A is a perspective view seen from above, and FIG. 1B is a perspective view seen from below. [Diagram 2] FIG. 2 is an exploded perspective view of the tape cartridge. [Diagram 3] FIG. 2 is an exploded cross-sectional side view of the tape cartridge. [Figure 4] FIG. 1 is a schematic cross-sectional side view of a tape reel according to an embodiment of the present technology; [Diagram 5] 1 is a schematic cross-sectional view illustrating the operation of a typical tape reel. [Figure 6] 6 is a schematic diagram of a main part of a magnetic tape, illustrating a problem associated with the deformation of the tape reel shown in FIG. 5. [Figure 7] 1 is a side cross-sectional view of a reel half that constitutes a tape reel according to an embodiment of the present technology. [Figure 8] 3 is an enlarged cross-sectional view of a main portion of a reel hub in the tape reel. FIG. [Figure 9] 5A to 5C are schematic cross-sectional views illustrating the operation of the tape reel. [Figure 10] 8 is a side cross-sectional view of a die device which is a manufacturing device for the reel half body shown in FIG. 7. [Figure 11] 11A to 11C are diagrams illustrating a method for measuring the gradient of the outer peripheral surface of a reel hub. [Figure 12] 11 is a diagram showing the results of measuring the gradient of the outer peripheral surface of a reel hub molded using the mold device shown in FIG. 10. FIG. [Figure 13] 6 is a diagram showing the results of measuring the gradient of the outer circumferential surface of the reel hub of the tape reel shown in FIG. 5. [Figure 14] FIG. 2 is a schematic diagram of a magnetic tape seen from the side. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Hereinafter, embodiments of the present technology will be described with reference to the drawings.
[0016] Fig. 1 is an overall perspective view of a tape cartridge 1 according to an embodiment of the present technology, where A is a perspective view seen from the top (upper shell 2) side, and B is a perspective view seen from the bottom (lower shell 3) side. Fig. 2 is an exploded perspective view of the tape cartridge 1, and Fig. 3 is an exploded side cross-sectional view thereof.
[0017] [Overall configuration of tape cartridge] The tape cartridge 1 of this embodiment has a configuration in which a single tape reel 5 around which a magnetic tape 22 is wound is rotatably housed inside a cartridge case 4 formed by joining an upper shell 2 and a lower shell 3 with a plurality of screw members. The tape cartridge 1 of this embodiment will be described below using a magnetic tape cartridge conforming to the LTO (Linear Tape Open) standard as an example.
[0018] The tape reel 5 has a cylindrical reel hub 6 with a bottom, a lower flange 7 integrally formed with the lower end of the reel hub 6, and an upper flange 8 joined to the upper end of the reel hub 6, each of which is formed from an injection molded synthetic resin material.
[0019] 1B, a chucking gear 9 is formed in an annular shape at the center of the underside of the tape reel 5, which engages with the reel rotation drive shaft of the tape drive device, and is exposed to the outside through an opening 10 provided in the center of the lower shell 3. On the inner periphery of this chucking gear 9, an annular metal plate 11 that is magnetically attracted to the reel rotation drive shaft is fixed to the bottom outer surface of the reel hub 6 by insert molding.
[0020] A reel lock mechanism is provided inside the reel hub 6 to prevent the tape reel 5 from rotating when the tape cartridge 1 is not in use. As shown in Fig. 3, the reel lock mechanism includes a plurality of gear-forming walls 12 erected on the upper surface of the bottom 60 of the reel hub 6, a reel lock member 13 having engagement teeth 13a that mesh with a gear portion 12a formed on the upper surface of the gear-forming walls 12, a reel lock release member 14 for releasing the engagement between the gear-forming walls 12 and the reel lock member 13, and a reel spring 15 provided between the inner surface of the upper shell 2 and the upper surface of the reel lock member 13. The reel spring 15 is a coil spring, and biases the tape reel 5 towards the lower shell 3 via the reel lock member 13.
[0021] The gear forming wall 12 has an arc shape and is formed on the upper surface of the bottom portion 60 of the reel hub 6 at three equally spaced locations on the same circumference around the axis of the reel hub 6. The engagement teeth 13a of the reel lock member 13 that face the gear portion 12a of the gear forming wall 12 are formed in an annular shape on the lower surface of the reel lock member 13 and are constantly biased in the direction of engagement with the gear portion 12a by receiving a reel spring 15. A mating protrusion 13c is formed on the upper surface of the reel lock member 13, and a mating recess 2a that fits into the mating protrusion 13c is formed in the approximate center of the inner surface of the upper shell 2.
[0022] The reel lock release member 14 has a generally triangular shape and is disposed between the bottom 60 of the reel hub 6 and the reel lock member 13. A total of three legs 14a are formed on the underside of the reel lock release member 14, protruding downward from each apex of the generally triangular shape, and these legs are positioned between the gears of the chucking gear 9 via insertion holes 6a formed in the bottom 60 of the reel hub 6 when the cartridge is not in use.
[0023] When the cartridge is in use, each leg 14a of the reel lock release member 14 is pressed upward by the reel rotation drive shaft of the tape drive device which engages with the chucking gear 9, thereby moving the reel lock member 13 to the unlocked position against the biasing force of the reel spring 15. The reel lock release member 14 is configured to be rotatable relative to the reel lock member 13 together with the tape reel 5. A support surface 14b is provided at approximately the center of the upper surface of the reel lock release member 14 to support a sliding contact portion 13b having an arc-shaped cross section and formed to protrude from approximately the center of the lower surface of the reel lock member 13.
[0024] One side wall 26 of the cartridge case 4 is provided with a draw-out opening 27 for drawing out one end of the magnetic tape 22 to the outside. A slide door 29 for opening and closing the draw-out opening 27 is disposed inside the side wall 26. The slide door 29 is configured to slide in a direction to open the draw-out opening 27 against the biasing force of a torsion spring 57 by engaging with a tape loading mechanism (not shown) of the tape drive device.
[0025] A leader pin 31 is fixed to one end of the magnetic tape 22. The leader pin 31 is configured to be detachable from a pin holding portion 33 provided on the inside side of the drawing outlet 27. The pin holding portions 33 are attached to the inner surfaces of the upper shell 2 and the lower shell 3, respectively, and are configured to be able to elastically hold the upper end and the lower end of the leader pin 31, respectively.
[0026] Inside the cartridge case 4, there is disposed a safety tab 25 for preventing accidental erasure of information recorded on the magnetic tape 22, as well as a cartridge memory 54 capable of contactlessly reading and writing contents related to the information recorded on the magnetic tape 22. The cartridge memory 54 is constituted by a contactless communication medium having an antenna coil, an IC chip, etc. mounted on a substrate.
[0027] [Tape reel] Next, the tape reel 5 will be described in detail.
[0028] As described above, the tape reel 5 has a reel hub 6, a lower flange 7 as a first flange, and an upper flange 8 as a second flange. In this embodiment, the lower flange 7 is integrally formed with the lower end (first end) of the reel hub 6, and the upper flange 8 is joined to the upper end (second end) of the reel hub 6 by ultrasonic bonding or the like. The reel hub 6 has a generally cylindrical shape, and its axial height is slightly larger than the width (12.65 mm) of the magnetic tape 22, being approximately 13 mm (12.87 mm). The inner diameter of the reel hub 6 is approximately 40 mm (39.6 mm), and its wall thickness, which is the thickness dimension in the radial direction, is approximately 2 mm.
[0029] The reel hub 6 and the lower flange 7 are integrally molded using synthetic resin materials such as PC (polycarbonate) and ABS (acrylonitrile butadiene styrene). The upper flange 8 is also molded using synthetic resin materials such as PC and ABS. The molding material for the reel hub 6 and the lower flange 7 may be a composite material in which an inorganic filler such as a glass filler is added to the above synthetic resin material for the purpose of improving strength. The weight ratio of the glass filler is not particularly limited, and is, for example, about 10% to 30% by weight of the base synthetic resin material. In this embodiment, a composite material containing 10% to 20% by weight of a glass filler in a polycarbonate resin is used as the molding material for the reel hub 6.
[0030] (Basic configuration of reel hub) 4 is a schematic side cross-sectional view of tape reel 5. Reel hub 6 has a cylindrical shape with a constant thickness from its lower end 6a, which is formed integrally with lower flange 7, to its upper end 6b, which is joined to upper flange 8. Upper flange 8 is positioned by fitting an annular protrusion 8b, which is formed along the periphery of an opening 8a provided in the center, into the inner circumferential surface of upper end 6b of reel hub 6. Reel hub 6 is ultrasonically joined to upper flange 8 directly above upper end 6b.
[0031] The outer peripheral surface 6c of the reel hub 6 functions as a winding surface on which the magnetic tape 22 is wound. The outer peripheral surface 6c is typically a flat cylindrical surface. The outer peripheral surface 6c of the reel hub 6 is pressed radially inward by the magnetic tape 22 being wound tightly (winding pressure). In a reel structure in which the reel hub 6 is integrally molded with the lower flange 7, the upper end 6b side of the reel hub 6 has lower rigidity than the lower end 6a side. As shown in a slightly exaggerated manner in FIG. 5, the winding pressure of the magnetic tape 22 acts as a pressing force that pushes the upper end 6b of the reel hub 8 radially inward (see arrow A). When the upper end 6b of the reel hub 6 is deformed radially inward by this pressing force, the difference in outer diameter between both ends of the reel hub 6 becomes large, and as shown typically in FIG. 6, the lower edge portion 22a of the magnetic tape 22 facing the lower flange 7 may be deformed to be longer than the upper edge 22b of the magnetic tape facing the upper flange 8. In this case, deformation wrinkles D are generated on the bottom edge 22a, which may cause insufficient contact between the area on the bottom edge side of the magnetic tape 22 and the drive head, making it impossible to stably read and write data.
[0032] In particular, in recent years, as the recording capacity of tape cartridges increases, the magnetic tape has become thinner and longer, so the winding pressure applied to the reel hub has been increasing. Furthermore, the winding pressure applied to the reel hub increases further due to the influence of long-term storage of tape cartridges in high-temperature and high-humidity environments, which makes it more likely that the deformation amount of the upper end portion 6b of the reel hub 6 will increase more and more.
[0033] The present inventors have found that by forming the outer circumferential surface of the reel hub 6 into a shape described below, rather than a flat cylindrical surface, it is possible to suppress deformation of the upper end portion 6b of the reel hub 6 due to the winding pressure of the magnetic tape 22. The details are described below.
[0034] (Outer surface shape of reel hub) FIG. 7 is a side cross-sectional view of a reel half 67 in which the reel hub 6 and the lower flange 7 are integrally formed according to this embodiment, and FIG. As shown in FIG. 7, the reel hub 6 has a lower end 6a (first end) formed integrally with the lower flange 7 (first flange), an upper end 6b (second end) to which the upper flange 8 is joined, an outer peripheral surface 6d around which the magnetic tape 22 is wound, and an inner peripheral surface 6e. The outer circumferential surface 6d of the reel hub 6 has a first outer circumferential region 6d1 and a second outer circumferential region 6d2, as shown in an enlarged view in Fig. 8. On the other hand, the inner circumferential surface 6e of the reel hub 6 typically has a flat cylindrical surface shape.
[0035] The first outer peripheral region 6d1 is a region that expands in diameter from the lower end 6a to the upper end 6b of the reel hub 6. The shape of the first outer peripheral region 6d1 is not particularly limited as long as it expands in diameter from the lower end 6a to the upper end 6b of the reel hub 6. For example, the first outer peripheral region 6d1 may be a linear tapered surface or may be formed of a curved surface. The shape of the curved surface may be a bulging surface that is convex toward the radially outward direction of the reel hub 6, a recessed surface that is convex toward the radially inward direction of the reel hub 6, or a composite curved surface that includes these bulging and recessed surfaces. In other words, the surface shape of the first outer peripheral region 6d1 can be arbitrarily adjusted according to the molding conditions of the reel hub 6 (molding material, molding temperature, surface properties of the molding die, etc.).
[0036] The second outer circumferential region 6d2 is a region that expands in diameter from the first outer circumferential region 6d1 to the upper end portion 6b of the reel hub 6, and forms a ridge portion 6d3 on the boundary with the first outer circumferential region 6d1.
[0037] The shape of the second outer peripheral region 6d2 is not particularly limited as long as it expands in diameter from the ridge portion 6d3 toward the upper end portion 6b of the reel hub 6. For example, the second outer peripheral region 6d2 may be a linear tapered surface or may be formed of a curved surface. The shape of the curved surface may be a bulging surface that is convex toward the radially outward direction of the reel hub 6, a recessed surface that is convex toward the radially inward direction of the reel hub 6, or a compound curved surface including these bulging and recessed surfaces. As with the first outer peripheral region 6d1, the surface shape of the second outer peripheral region 6d2 can be arbitrarily adjusted according to the molding conditions of the reel hub 6 (molding material, molding temperature, surface properties of the molding die, etc.).
[0038] The ridge portion 6d3 has a shape that protrudes radially outward of the reel hub 6. In other words, as shown in Fig. 8, if the taper angle of the first outer circumferential region 6d1 (the angle formed by the line segment connecting the ridge portion 6d3 and the outer circumferential edge portion P1 of the lower end portion 6a of the reel hub 6 with respect to the axis C1) is θ1, and the taper angle of the second outer circumferential region 6d2 (the angle formed by the line segment connecting the ridge portion 6d3 and the outer circumferential edge portion P2 of the upper end portion 6b of the reel hub 6 with respect to the axis C1) is θ2, the relationship θ1>θ2 is satisfied.
[0039] The ridge portion 6d3 corresponds to an inflection point that connects the first outer circumferential region 6d1 having a taper angle of θ1 and the second outer circumferential region 6d2 having a taper angle of θ2. The cross-sectional shape of the ridge portion 6d3 along the axis C1 is not particularly limited, and may be a corner portion formed between the first outer circumferential region 6d1 and the second outer circumferential region 6d2, or a curved surface formed between them.
[0040] By providing the first outer peripheral region 6d1 on the outer peripheral surface 6d of the reel hub 6, the radius of the lower end 6a of the reel hub 6 becomes smaller than the radius of the upper end 6b. In other words, the thickness of the lower end 6a can be made smaller than the thickness of the upper end 6b. Therefore, when the winding pressure of the magnetic tape 22 acts on the reel hub 6, or during long-term storage in a high-temperature and high-humidity environment, the reel hub 6 is easily deformed radially inward over its entire height direction due to bending stress with the connection area between the lower end 6a of the reel hub 6 and the lower flange 7 as a fulcrum. Therefore, the upper end 6b of the reel hub 6 is prevented from falling radially inward as shown in FIG. 5, and the central part of the height direction of the reel hub 6 can be deformed to have a curved shape that is convex radially inward as shown in FIG. 9. This makes it possible to reduce the difference in outer diameter between both ends of the reel hub 6, thereby preventing the occurrence of deformation wrinkles as shown in FIG. 6 on the lower edge part 22a of the magnetic tape 22 and ensuring stable recording and reproducing characteristics of the magnetic tape 22.
[0041] Furthermore, by providing the second outer peripheral region 6d2 on the outer peripheral surface 6d of the reel hub 6, the difference in outer diameter between the lower end 6a and the upper end 6b of the reel hub 6 can be kept within a certain range. This makes it possible to suppress disturbance in the winding shape of the magnetic tape 22 when starting to wind the magnetic tape 22 around the reel hub 6, and to reduce damage to the edge of the magnetic tape 22 due to interference with the lower flange 7 or the upper flange 8.
[0042] Furthermore, by providing the second outer circumferential region 6d2 on the outer circumferential surface 6d of the reel hub 6, the second outer circumferential region 6d2 of the reel hub 6 can be brought closer to a state parallel to the axis C1 when the reel hub 6 is deformed due to the winding pressure of the magnetic tape 22. This makes the winding shape of the magnetic tape 22 more stable, and makes it possible to further reduce damage to the edge portions of the magnetic tape 22.
[0043] Here, it is preferable that the ridge portion 6d3 is located closer to the lower end portion 6a of the reel hub 6 than the center of the height H (12.87 mm) of the reel hub 6. In this embodiment, the height H1 from the lower end portion 6a of the reel hub 6 is 3 mm or more and 5 mm or less. If the height H1 is less than 3 mm, the above-mentioned action of this embodiment may not be effectively achieved. If the height H1 exceeds 5 mm, the releasability of the molding die for forming the outer circumferential surface 6d of the reel hub 6 may decrease, as described later. By setting the height H1 to 3 mm or more and 5 mm or less, it is possible to ensure good moldability of the reel hub 6 while preventing deformation (see FIG. 5) in which the upper end portion 6b of the reel hub 6 falls radially inward during long-term storage of the tape cartridge 1 in a high-temperature and high-humidity environment.
[0044] In this embodiment, as shown in Fig. 8, the difference ΔR1 between the radius of the ridgeline portion 6d3 centered on the axis C1 and the radius of the outer circumferential edge portion P1 is 5 µm or more and 25 µm or less. In other words, the difference between the outer diameter of the ridgeline portion 16d3 and the outer diameter of the bottom end portion 6a of the reel hub 6 is 10 µm or more and 50 µm or less. This allows the ridgeline portion 6d3 to be stably formed at the position of height H1.
[0045] Furthermore, the difference ΔR2 between the radius of the lower end 6a of the reel hub 6 and the radius of the upper end 6b of the reel hub 6 about the axis C1 is 15 μm or more and 45 μm or less. In other words, the difference between the outer diameter of the lower end 6a of the reel hub 6 and the outer diameter of the upper end 6a of the reel hub 6 is 30 μm or more and 90 μm or less. This makes it possible to effectively prevent the upper end 6b of the reel hub 6 from falling radially inward during long-term storage of the tape cartridge 1 in a high-temperature, high-humidity environment.
[0046] The magnitudes of the height H1 and the radius differences ΔR1 and ΔR2 are not limited to the above examples, and can be set arbitrarily depending on the height, thickness, and type of molding material of the reel hub 6. For example, when a synthetic resin material containing glass filler is used as the molding material, the rigidity of the reel hub 6 changes depending on the type of synthetic resin material, the amount of glass filler contained, and other factors. For this reason, it is preferable to optimize each of the above dimensions depending on the rigidity of the reel hub 6.
[0047] [Reel hub manufacturing equipment] Fig. 10 is a side cross-sectional view of a die assembly 70 which is a manufacturing device for the reel half 67 shown in Fig. 7. The die assembly 70 has a first die 71 which forms the outer peripheral surface 6d of the reel hub 6 and the inner surface of the lower flange 7, a second die 72 which forms the inner peripheral surface 6e of the reel hub 6 and the inner bottom surface of the reel hub 6, and a third die 73 which forms the outer surface of the lower flange 7.
[0048] The first mold 71 forms a cavity 70C into which a molding material is filled, between the second mold 72 and the third mold 73. The first mold 71 has a first molding surface 711 that forms the first outer circumferential region 6d1 of the reel hub 6, a second molding surface 712 that forms the second outer circumferential region 6d2 of the reel hub 6, a third molding surface that forms the inner surface of the lower flange 7, and a fourth molding surface 714 that forms the upper end portion 6b of the reel hub 6.
[0049] First molding surface 711 is a tapered surface shaped like an inverted truncated cone inclined at an angle θ1 with respect to axis C2. Second molding surface 712 is a cylindrical surface parallel to axis C2. In this embodiment, height H2 of first molding surface 711 is 3 μm or more and 5 μm or less. Difference ΔT between the minimum radius of first molding surface 711 (the radius of the lower end of first molding surface 711) and the maximum radius of first molding surface 711 (the radius of second molding surface 712) centered on axis C2 is 7 μm or more and 15 μm or less.
[0050] This allows the first outer peripheral region 6d1 to be stably formed in the shape shown in Fig. 8. If H2 exceeds 5 µm and ΔT exceeds 15 µm, the releasability of the first mold 71 using the thermal contraction of the first outer peripheral region 6d1 after molding may be impaired. Therefore, it is preferable to appropriately adjust the upper limits of these values depending on the type of molding material used.
[0051] The reel half 67 is molded by injecting a molding material (a composite material of polycarbonate and glass filler) into the cavity 70C through a gate (not shown). This allows the formation of a reel hub 6 having an outer circumferential surface 6d including a first outer circumferential region 6d1 and a second outer circumferential region 6d2 as shown in Figure 7. Furthermore, due to thermal contraction of the molding material after molding, the second outer circumferential region 6d2 formed by the second molding surface 712 becomes an inclined surface having a taper angle θ2 as shown in Figure 8.
[0052] The present inventors measured the gradient of the outer peripheral surface 6d of the molded reel hub 6 as shown in Fig. 11. The measuring machine used was "Mitutoyo Roundtest RA-2100" manufactured by Mitutoyo Corporation. The measurement procedure was as follows.
[0053] First, the chucking gear 9 (see FIG. 1B) at the bottom of the reel hub 6 was set on a jig (master gear) on a rotating table (not shown), and the reel half 67 was rotatably supported. With the reel half 67 stopped, a probe 81 (diameter 1.6 mm) was brought into contact with the outer circumferential surface 6d of the reel hub 6, and the probe 81 was traced up and down to measure the gradient of the outer circumferential surface 6d. In order to avoid damaging the probe 81, the origin of the measurement was set at a position 1 mm above the bottom end 6a of the reel hub 6, and the measurement length was set to 11 mm. After tracing with the probe 81, the rotary table was rotated 30° and the same measurement as above was then performed. This operation was repeated 12 times to perform measurements at 12 locations in the circumferential direction of the reel hub 6. The average value of the measured waveforms at the 12 locations is shown in Figure 12 (left side of the figure) as a gradient waveform TR1.
[0054] Next, the upper flange 8 was joined to the reel half 67 to prepare the tape reel 5, and then the magnetic tape 22 of 1000 m in length was wound around the tape reel 5 with a tension of 0.55 N to prepare the tape cartridge 1. The tape cartridge 1 was stored for one week in a thermostatic chamber maintained at a temperature of 49°C and a relative humidity of 80%, which were the acceleration test conditions. Thereafter, the tape cartridge 1 was left in a normal temperature environment with a temperature of 23°C±2°C and a relative humidity of 40-60% for 24 hours. The tape reel 5 was then removed from the tape cartridge 1, and the gradient of the outer circumferential surface of the reel hub 6 after removing the magnetic tape 22 was measured in the same manner as described above. The result is shown as a gradient waveform TR2 in FIG. 12 (right side in the figure).
[0055] Immediately after molding, the gradient waveform TR1 of the outer circumferential surface 6d of the reel hub 6 had an inflection point of the inclination angle corresponding to the ridge line 6d3 (see FIG. 8) at the boundary between the first region 6d1 and the second gradient region 6d2 (see the region indicated by circle A in FIG. 12). In addition, the difference in radius between both ends (6a, 6b) of the reel hub 6 was approximately 35 μm.
[0056] On the other hand, according to the gradient waveform TR2 of the outer peripheral surface 6d of the reel hub 6 after the accelerated test, it was confirmed that the upper end 6b of the reel hub 6 was prevented from falling radially inward, and the intermediate region between the lower end 6a and the upper end 6b was deformed so as to be curved radially inward. In addition, the difference between the radius of the upper end 6b and the radius of the lower end 6a of the reel hub 6 was about 7 μm. Furthermore, the inventors have confirmed through experiments that in order to prevent deformation wrinkles at the edge of the magnetic tape 22 caused by deformation of the reel hub 6, it is preferable that the radius difference of the reel hub 6 after the acceleration test be 10 μm or less.
[0057] As a comparative example, Fig. 13 shows the results of measuring the gradient waveform of the hub outer peripheral surface using a method similar to that described above for a reel hub having an outer peripheral surface 6c (see Fig. 4) consisting of a flat cylindrical surface without a first outer peripheral region 6d1 and a second outer peripheral region 6d2. In Fig. 13, the left side shows the gradient waveform TR3 of the outer peripheral surface 6c immediately after molding, and the right side shows the gradient waveform TR4 of the outer peripheral surface 6c after the above-mentioned acceleration test. As shown in the figure, the radius difference between both ends of the reel hub after the acceleration test was 25μm to 30μm.
[0058] [Magnetic tape details] Next, the magnetic tape 22 used in this embodiment will be described in detail. Fig. 14 is a schematic side view of the magnetic tape 22. As shown in Fig. 14, the magnetic tape 22 is configured in a tape shape that is long in the longitudinal direction (X-axis direction), short in the width direction (Y-axis direction), and thin in the thickness direction (Z-axis direction).
[0059] The magnetic tape 22 includes a tape-shaped substrate 41 that is long in the longitudinal direction (X-axis direction), an underlayer (non-magnetic layer) 42 provided on one main surface of the substrate 41, a magnetic layer 43 provided on the underlayer 42, and a back layer 44 provided on the other main surface of the substrate 41. Note that the back layer 44 may be provided as necessary, and may be omitted. The magnetic tape 22 may be a perpendicular recording type magnetic recording medium or a longitudinal recording type magnetic recording medium.
[0060] The magnetic tape 22 has a long tape shape, and runs in the longitudinal direction during recording and reproduction. The surface of the magnetic layer 43 is the surface on which a magnetic head of a recording and reproduction device (not shown) runs. The magnetic tape 22 is preferably used in a recording and reproduction device equipped with a ring-type head as a recording head. The magnetic tape 22 is preferably used in a recording and reproduction device configured to be capable of recording data with a data track width of 1500 nm or less or 1000 nm or less.
[0061] (base material) The substrate 41 is a non-magnetic support that supports the underlayer 42 and the magnetic layer 43. The substrate 41 has a long film shape. The upper limit of the average thickness of the substrate 41 is preferably 4.2 μm or less, more preferably 3.8 μm or less, and even more preferably 3.4 μm or less. When the upper limit of the average thickness of the substrate 41 is 4.2 μm or less, the recording capacity that can be recorded in one data cartridge can be increased compared to that of a general magnetic tape. The lower limit of the average thickness of the substrate 41 is preferably 3 μm or more, more preferably 3.2 μm or more. When the lower limit of the average thickness of the substrate 41 is 3 μm or more, a decrease in the strength of the substrate 41 can be suppressed.
[0062] The average thickness of the substrate 41 is obtained as follows. First, a 1 / 2 inch wide magnetic tape 22 is prepared and cut to a length of 250 mm to prepare a sample. Next, layers other than the substrate 41 of the sample (i.e., the underlayer 42, the magnetic layer 43, and the back layer 44) are removed with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. Next, the thickness of the sample (substrate 41) is measured at five or more positions using a Mitutoyo Laser Hologram (LGH-110C) as a measuring device, and the measured values are simply averaged (arithmetic average) to calculate the average thickness of the substrate 41. Note that the measurement positions are selected randomly from the sample.
[0063] The substrate 41 contains polyester. By including polyester in the substrate 41, it is possible to reduce the Young's modulus in the longitudinal direction of the substrate 41. Therefore, by adjusting the tension in the longitudinal direction of the magnetic tape 22 during running by the recording and reproducing device, it is possible to keep the width of the magnetic tape 22 constant or approximately constant.
[0064] The polyester includes, for example, at least one of polyethylene terephthalate (PET), polyethylene naphthalate (PEN), polybutylene terephthalate (PBT), polybutylene naphthalate (PBN), polycyclohexylene dimethylene terephthalate (PCT), polyethylene-p-oxybenzoate (PEB), and polyethylene bisphenoxycarboxylate. When the substrate 41 includes two or more types of polyester, the two or more types of polyester may be mixed, copolymerized, or laminated. At least one of the terminals and side chains of the polyester may be modified.
[0065] The inclusion of polyester in the substrate 41 can be confirmed, for example, as follows. First, in the same manner as in the measurement of the average thickness of the substrate 41, layers of the sample other than the substrate 41 are removed. Next, an IR spectrum of the sample (substrate 41) is obtained by infrared absorption spectrometry (IR). Based on this IR spectrum, it can be confirmed that the substrate 41 contains polyester.
[0066] The base material 41 may further include at least one of polyamide, polyetheretherketone, polyimide, and polyamideimide, other than polyester, or may further include at least one of polyamide, polyimide, polyamideimide, polyolefins, cellulose derivatives, vinyl resins, and other polymer resins. The polyamide may be an aromatic polyamide (aramid). The polyimide may be an aromatic polyimide. The polyamideimide may be an aromatic polyamideimide.
[0067] When the base material 41 contains a polymer resin other than polyester, it is preferable that the base material 41 contains polyester as a main component. Here, the main component means the component with the largest content (mass ratio) among the polymer resins contained in the base material 41. When the base material 41 contains a polymer resin other than polyester, the polyester and the polymer resin other than polyester may be mixed or copolymerized.
[0068] The substrate 41 may be biaxially stretched in the longitudinal direction and the width direction. The polymer resin contained in the substrate 41 is preferably oriented in a direction oblique to the width direction of the substrate 41.
[0069] (magnetic layer) The magnetic layer 43 is a recording layer for recording signals by magnetization patterns. The magnetic layer 43 may be a perpendicular recording type recording layer or a longitudinal recording type recording layer. The magnetic layer 43 includes, for example, a magnetic powder, a binder, and a lubricant. The magnetic layer 43 may further include at least one additive selected from antistatic agents, abrasives, hardeners, rust inhibitors, and non-magnetic reinforcing particles, as necessary. The magnetic layer 43 is not limited to being composed of a coating film of a magnetic material, and may be composed of a sputtered film or a vapor deposition film of a magnetic material.
[0070] The arithmetic mean roughness Ra of the surface of the magnetic layer 43 is 2.0 nm or less, preferably 1.8 nm or less, and more preferably 1.6 nm or less. When the arithmetic mean roughness Ra is 2.0 nm or less, the output reduction due to spacing loss can be suppressed, and therefore excellent electromagnetic conversion characteristics can be obtained. The lower limit of the arithmetic mean roughness Ra of the surface of the magnetic layer 43 is preferably 1.0 nm or more, and more preferably 1.2 nm or more. When the lower limit of the arithmetic mean roughness Ra of the surface of the magnetic layer 43 is 1.0 nm or more, the decrease in running performance due to increased friction can be suppressed.
[0071] The arithmetic mean roughness Ra is obtained as follows. First, the surface of the magnetic layer 43 is observed by an AFM (Atomic Force Microscope) to obtain an AFM image of 40 μm×40 μm. The AFM is a Nano Scope IIIa D3100 manufactured by Digital Instruments, and the cantilever is made of single crystal silicon (Note 1). Measurements are performed with a tapping frequency of 200 to 400 Hz. Next, the AFM image is divided into 512×512 (=262,144) measurement points, and the height Z(i) (i: measurement point number, i=1 to 262,144) is measured at each measurement point. The heights Z(i) of each measurement point are simply averaged (arithmetic average) to obtain the average height (average surface) Zave (=(Z(1)+Z(2)+···+Z(262,144)) / 262,144). Next, the deviation Z"(i) (=Z(i)-Zave) from the average center line at each measurement point is found, and the arithmetic mean roughness Ra [nm] (=(Z"(1)+Z"(2)+···+Z"(262,144)) / 262,144) is calculated. In this case, the image is filtered using Flatten order 2 and planefit order 3 XY before being used as the data. (Note 1) Nano World SPM probe NCH normal type PointProbe L (Cantilever length) = 125 μm
[0072] The average thickness t of the magnetic layer 43 m The upper limit of the average thickness t of the magnetic layer 43 is 80 nm or less, preferably 70 nm or less, and more preferably 50 nm or less. m If the upper limit value is 80 nm or less, when a ring-type head is used as the recording head, the influence of the demagnetizing field can be reduced, and therefore further excellent electromagnetic conversion characteristics can be obtained.
[0073] The average thickness t of the magnetic layer 43 m The lower limit of the average thickness t of the magnetic layer 43 is preferably 35 nm or more. mIf the lower limit is 35 nm or more, when an MR type head is used as the reproducing head, output can be ensured, and therefore even better electromagnetic conversion characteristics can be obtained.
[0074] The average thickness t of the magnetic layer 43 m is obtained as follows. First, the magnetic tape 22 to be measured is processed by the FIB method or the like to be sliced. When the FIB method is used, a carbon layer and a tungsten layer are formed as protective films as a pretreatment for observing a TEM image of the cross section described later. The carbon layer is formed by a deposition method on the surface of the magnetic tape 22 on the magnetic layer 43 side and on the surface of the back layer 44 side, and the tungsten layer is further formed by a deposition method or a sputtering method on the surface on the magnetic layer 43 side. The slice is performed along the length direction (longitudinal direction) of the magnetic tape 22. That is, the slice forms a cross section parallel to both the longitudinal direction and the thickness direction of the magnetic tape 22.
[0075] The cross section of the obtained sliced sample is observed under the following conditions with a transmission electron microscope (TEM) to obtain a TEM image. Note that the magnification and acceleration voltage may be appropriately adjusted depending on the type of device. Equipment: TEM (Hitachi H9000NAR) Acceleration voltage: 300 kV Magnification: 100, 000x
[0076] Next, using the obtained TEM image, the thickness of the magnetic layer 43 is measured at at least 10 positions in the longitudinal direction of the magnetic tape 22. The obtained measured values are simply averaged (arithmetic average) to obtain an average thickness t m The positions at which the above measurements are performed are to be selected randomly from the test piece.
[0077] (magnetic powder) The magnetic powder includes a plurality of magnetic particles. The magnetic particles are, for example, particles containing hexagonal ferrite (hereinafter referred to as "hexagonal ferrite particles"), particles containing epsilon iron oxide (ε iron oxide) (hereinafter referred to as "ε iron oxide particles"), or particles containing Co-containing spinel ferrite (hereinafter referred to as "cobalt ferrite particles"). It is preferable that the magnetic powder has a crystal orientation preferentially in the thickness direction (perpendicular direction) of the magnetic tape 22.
[0078] (Hexagonal ferrite particles) The hexagonal ferrite particles have a plate shape, such as a hexagonal plate shape. In this specification, the hexagonal slope shape includes an almost hexagonal slope shape. The hexagonal ferrite preferably contains at least one of Ba, Sr, Pb and Ca, more preferably at least one of Ba and Sr. The hexagonal ferrite may be, specifically, for example, barium ferrite or strontium ferrite. The barium ferrite may further contain at least one of Sr, Pb and Ca in addition to Ba. The strontium ferrite may further contain at least one of Ba, Pb and Ca in addition to Sr.
[0079] More specifically, hexagonal ferrite has the general formula MFe 12 O 19 The average composition is represented by the formula: where M is, for example, at least one metal selected from Ba, Sr, Pb, and Ca, and preferably at least one metal selected from Ba and Sr. M may be a combination of Ba and at least one metal selected from the group consisting of Sr, Pb, and Ca. M may also be a combination of Sr and at least one metal selected from the group consisting of Ba, Pb, and Ca. In the above general formula, a part of Fe may be substituted with another metal element.
[0080] When the magnetic powder contains hexagonal ferrite particles, the average particle size of the magnetic powder is preferably 30 nm or less, more preferably 12 nm to 25 nm, even more preferably 12 nm to 22 nm, particularly preferably 12 nm to 19 nm, and most preferably 12 nm to 16 nm. When the average particle size of the magnetic powder is 30 nm or less, it is possible to obtain even better electromagnetic conversion characteristics (e.g., SNR) in a high recording density magnetic tape 22. On the other hand, when the average particle size of the magnetic powder is 12 nm or more, the dispersibility of the magnetic powder is further improved, and even better electromagnetic conversion characteristics (e.g., SNR) can be obtained.
[0081] The average aspect ratio of the magnetic powder is preferably 1.0 or more and 3.0 or less, more preferably 1.3 or more and 2.8 or less, and even more preferably 1.6 or more and 2.7 or less. When the average aspect ratio of the magnetic powder is within the range of 1.0 or more and 2.5 or less, aggregation of the magnetic powder can be suppressed. In addition, when the magnetic powder is vertically oriented in the process of forming the magnetic layer 43, the resistance applied to the magnetic powder can be suppressed. Therefore, the vertical orientation of the magnetic powder can be improved.
[0082] When the magnetic powder contains hexagonal ferrite particles, the average particle size and the average aspect ratio of the magnetic powder are obtained as follows. First, the magnetic tape 22 to be measured is processed by the FIB method or the like to be thinned. When the FIB method is used, a carbon layer and a tungsten layer are formed as protective films as a pretreatment for observing a TEM image of the cross section described later. The carbon layer is formed by a deposition method on the surface of the magnetic tape 22 on the magnetic layer 43 side and on the surface of the back layer 44 side, and the tungsten layer is further formed by a deposition method or a sputtering method on the surface on the magnetic layer 43 side. The thinning is performed along the length direction (longitudinal direction) of the magnetic tape 22. That is, the thinning forms a cross section parallel to both the longitudinal direction and the thickness direction of the magnetic tape 22.
[0083] The cross section of the obtained thin sample is observed using a transmission electron microscope (H-9500 manufactured by Hitachi High-Technologies Corporation) at an acceleration voltage of 200 kV and a total magnification of 500,000 times, so that the entire magnetic layer 43 is included in the thickness direction of the magnetic layer 43, and a TEM photograph is taken. Next, from the TEM photograph taken, 50 particles are selected whose side faces the observation surface direction and whose particle thickness can be clearly confirmed. The maximum plate thickness DA of each of the selected 50 particles whose thickness can be clearly confirmed is measured. The maximum plate thicknesses DA thus obtained are simply averaged (arithmetic mean) to obtain the average maximum plate thickness DA ave Next, the plate diameter DB of each magnetic powder is measured. To measure the plate diameter DB of the particles, 50 particles whose plate diameters can be clearly confirmed are selected from the TEM photograph. The plate diameter DB of each of the selected 50 particles is measured. The plate diameters DB thus obtained are simply averaged (arithmetic average) to obtain the average plate diameter DB ave Calculate the average plate diameter DB ave is the average grain size. And the average maximum plate thickness DA ave and average plate diameter DB ave The average aspect ratio of the particles (DB ave / DA ave ) is required.
[0084] When the magnetic powder comprises hexagonal ferrite particles, the average particle volume of the magnetic powder is preferably 3400 nm 3 Less than or equal to 400 nm, more preferably 3 More than 2600nm 3 Less than or equal to 400 nm, and even more preferably 3 More than 1700nm 3 Below 400 nm, particularly preferably 3 More than 1200nm 3 Below 400 nm, most preferably 3 More than 1000nm 3 The average particle volume of the magnetic powder is 3400 nm or less. 3 If the average particle size of the magnetic powder is 25 nm or less, the same effect as when the average particle volume of the magnetic powder is 500 nm or less can be obtained. 3If the average particle size of the magnetic powder is 12 nm or more, the same effect as in the case where the average particle size of the magnetic powder is 12 nm or more can be obtained.
[0085] The average particle volume of the magnetic powder can be calculated as follows. First, as described above in relation to the method for calculating the average particle size of the magnetic powder, the average major axis length DA ave and average plate diameter DB ave Next, calculate the average volume V of the magnetic powder using the following formula:
number
[0086] (ε iron oxide particles) The ε iron oxide particles are hard magnetic particles that can obtain high coercive force even in the case of fine particles. The ε iron oxide particles are spherical or cubic. In this specification, the term "spherical" includes "approximately spherical". Furthermore, the term "cubic" includes "approximately cubic". Since the ε iron oxide particles have the above-mentioned shape, when the ε iron oxide particles are used as the magnetic particles, the contact area between the particles in the thickness direction of the magnetic tape 22 can be reduced and the aggregation between the particles can be suppressed compared to when hexagonal plate-shaped barium ferrite particles are used as the magnetic particles. Therefore, the dispersibility of the magnetic powder can be improved, and further excellent electromagnetic conversion characteristics (e.g., SNR) can be obtained.
[0087] The ε-iron oxide particles have a core-shell structure. Specifically, the ε-iron oxide particles have a core and a two-layered shell portion provided around the core. The two-layered shell portion has a first shell portion provided on the core and a second shell portion provided on the first shell portion.
[0088] The core portion contains ε-iron oxide. The ε-iron oxide contained in the core portion is ε-Fe 2 O 3 It is preferable that the main phase is a crystal, and more preferable that it is made of a single phase ε-Fe2O3.
[0089] The first shell portion covers at least a part of the periphery of the core portion. Specifically, the first shell portion may cover a part of the periphery of the core portion, or may cover the entire periphery of the core portion. From the viewpoint of ensuring sufficient exchange coupling between the core portion and the first shell portion and improving magnetic properties, it is preferable that the first shell portion covers the entire surface of the core portion.
[0090] The first shell portion is a so-called soft magnetic layer, and contains a soft magnetic material such as α-Fe, a Ni-Fe alloy, an Fe-Si-Al alloy, etc. The α-Fe may be obtained by reducing ε-iron oxide contained in the core portion.
[0091] The second shell portion is an oxide coating as an oxidation prevention layer. The second shell portion includes α-iron oxide, aluminum oxide, or silicon oxide. The α-iron oxide is, for example, Fe 3 O 4 , Fe 2 O 3 and FeO. When the first shell portion contains α-Fe (soft magnetic material), the α-iron oxide may be obtained by oxidizing the α-Fe contained in the first shell portion.
[0092] By having the ε iron oxide particles have the first shell portion as described above, the coercivity Hc of the core portion alone can be kept large to ensure thermal stability, while the coercivity Hc of the ε iron oxide particles (core-shell particles) as a whole can be adjusted to a coercivity Hc suitable for recording. Furthermore, by having the ε iron oxide particles have the second shell portion as described above, it is possible to prevent the ε iron oxide particles from being exposed to air during and before the manufacturing process of the magnetic tape 22, which would cause rust or the like to form on the particle surface, thereby preventing the properties of the ε iron oxide particles from deteriorating. Therefore, it is possible to prevent the properties of the magnetic tape 22 from deteriorating.
[0093] The ε-iron oxide particles may have a shell part with a single layer structure. In this case, the shell part has the same structure as the first shell part. However, from the viewpoint of suppressing deterioration of the properties of the ε-iron oxide particles, it is preferable that the ε-iron oxide particles have a shell part with a two-layer structure, as described above.
[0094] The ε iron oxide particles may contain an additive instead of the core-shell structure, or may have a core-shell structure and contain an additive. In this case, part of the Fe in the ε iron oxide particles is replaced with the additive. By containing an additive in the ε iron oxide particles, the coercive force Hc of the ε iron oxide particles as a whole can be adjusted to a coercive force Hc suitable for recording, thereby improving ease of recording. The additive is a metal element other than iron, preferably a trivalent metal element, more preferably at least one of Al, Ga and In, and even more preferably at least one of Al and Ga.
[0095] Specifically, ε-iron oxide containing additives is ε-Fe 2-x M x O 3 crystal (wherein M is a metal element other than iron, preferably a trivalent metal element, more preferably at least one of Al, Ga and In, and even more preferably at least one of Al and Ga. x is, for example, 0 <x<1である。)である。
[0096] The average particle size (average maximum particle size) of the magnetic powder is, for example, 22 nm or less. The average particle size (average maximum particle size) of the magnetic powder is preferably 20 nm or less, more preferably 8 nm or more and 20 nm or less, even more preferably 10 nm or more and 18 nm or less, particularly preferably 10 nm or more and 16 nm or less, and most preferably 10 nm or more and 14 nm or less. In the magnetic tape 22, an area having a size of 1 / 2 the recording wavelength becomes an actual magnetized area. Therefore, by setting the average particle size of the magnetic powder to be half or less of the shortest recording wavelength, it is possible to obtain even better electromagnetic conversion characteristics (e.g., SNR). Therefore, when the average particle size of the magnetic powder is 22 nm or less, it is possible to obtain even better electromagnetic conversion characteristics (e.g., SNR) in a high recording density magnetic tape 22 (e.g., a magnetic tape 22 configured to be able to record signals at the shortest recording wavelength of 44 nm or less). On the other hand, when the average particle size of the magnetic powder is 8 nm or more, the dispersibility of the magnetic powder is further improved, and even better electromagnetic conversion characteristics (e.g., SNR) can be obtained.
[0097] The average aspect ratio of the magnetic powder is preferably 1.0 or more and 3.0 or less, more preferably 1.0 or more and 2.5 or less, even more preferably 1.0 or more and 2.1 or less, and particularly preferably 1.0 or more and 1.8 or less. When the average aspect ratio of the magnetic powder is within the range of 1.0 or more and 3.0 or less, aggregation of the magnetic powder can be suppressed. In addition, when the magnetic powder is vertically oriented in the process of forming the magnetic layer 43, the resistance applied to the magnetic powder can be suppressed. Therefore, the vertical orientation of the magnetic powder can be improved.
[0098] When the magnetic powder contains ε iron oxide particles, the average particle size and the average aspect ratio of the magnetic powder are obtained as follows. First, the magnetic tape 22 to be measured is processed and sliced by FIB (Focused Ion Beam) method or the like. When the FIB method is used, a carbon layer and a tungsten layer are formed as protective layers as a pretreatment for observing a TEM image of the cross section described later. The carbon layer is formed by a deposition method on the surface of the magnetic tape 22 on the magnetic layer 43 side and on the surface of the back layer 44 side, and the tungsten layer is further formed by a deposition method or a sputtering method on the surface on the magnetic layer 43 side. The slice is performed along the length direction (longitudinal direction) of the magnetic tape 22. That is, the slice forms a cross section parallel to both the longitudinal direction and the thickness direction of the magnetic tape 22.
[0099] The cross section of the obtained thin sample is observed using a transmission electron microscope (H-9500 manufactured by Hitachi High-Technologies Corporation) at an acceleration voltage of 200 kV and a total magnification of 500,000 times so that the entire magnetic layer 43 is included in the thickness direction of the magnetic layer 43, and a TEM photograph is taken. Next, 50 particles whose particle shapes can be clearly confirmed are selected from the TEM photograph taken, and the long axis length DL and short axis length DS of each particle are measured. Here, the long axis length DL means the maximum distance between two parallel lines drawn from all angles so as to be tangent to the contour of each particle (so-called maximum Feret diameter). On the other hand, the short axis length DS means the maximum length of the particle in the direction perpendicular to the long axis (DL) of the particle. Next, the long axis lengths DL of the measured 50 particles are simply averaged (arithmetic average) to obtain the average long axis length DL ave The average major axis length DL ave is the average particle size of the magnetic powder. The short axis lengths DS of the 50 measured particles are simply averaged (arithmetic mean) to obtain the average short axis length DS ave Then, calculate the average major axis length DL ave and mean minor axis length DS ave The average aspect ratio of the particles (DL ave / DS ave ) is required.
[0100] The average particle volume of the magnetic powder is preferably 5600 nm 3 Less than or equal to 250 nm, preferably 3 More than 4200nm 3 Less than or equal to 600 nm, and even more preferably 3 More than 3000nm 3 Below 600 nm, particularly preferably 3 More than 2200nm 3 Below 600 nm, most preferably 3 More than 1500nm 3 Generally, the noise of the magnetic tape 22 is inversely proportional to the square root of the number of particles (i.e., proportional to the square root of the particle volume), so by making the particle volume smaller, it is possible to obtain better electromagnetic conversion characteristics (e.g., SNR). Therefore, when the average particle volume of the magnetic powder is 5600 nm 3 When the average particle size of the magnetic powder is 22 nm or less, it is possible to obtain even better electromagnetic conversion characteristics (e.g., SNR), as in the case where the average particle size of the magnetic powder is 22 nm or less. 3 If the average particle size of the magnetic powder is 8 nm or more, the same effect as in the case where the average particle size of the magnetic powder is 8 nm or more can be obtained.
[0101] When the ε iron oxide particles are spherical, the average particle volume of the magnetic powder can be calculated as follows. First, the average major axis length DL is calculated in the same manner as in the above-mentioned method for calculating the average particle size of the magnetic powder. ave Next, calculate the average volume V of the magnetic powder using the following formula: V = (π / 6) × DL ave 3
[0102] When the ε iron oxide particles have a cubic shape, the average volume of the magnetic powder is obtained as follows. The magnetic tape 22 is processed and sliced by a FIB (Focused Ion Beam) method or the like. When the FIB method is used, a carbon film and a tungsten thin film are formed as protective films as a pretreatment for observing a TEM image of the cross section described later. The carbon film is formed by a deposition method on the surface of the magnetic tape 22 on the magnetic layer 43 side and on the surface of the back layer 44 side, and the tungsten thin film is further formed by a deposition method or a sputtering method on the surface on the magnetic layer 43 side. The slice is performed along the length direction (longitudinal direction) of the magnetic tape 22. That is, the slice forms a cross section parallel to both the longitudinal direction and the thickness direction of the magnetic tape 22.
[0103] The obtained thin sample is observed in cross section in the thickness direction of the magnetic layer 43, using a transmission electron microscope (H-9500 manufactured by Hitachi High-Technologies Corporation) at an acceleration voltage of 200 kV and a total magnification of 500,000 times, so that the entire magnetic layer 43 is included, and a TEM photograph is obtained. The magnification and acceleration voltage may be adjusted appropriately depending on the type of device. Next, 50 particles whose particle shapes are clear are selected from the TEM photograph, and the side length DC of each particle is measured. Next, the side lengths DC of the measured 50 particles are simply averaged (arithmetic mean) to obtain the average side length DC ave Next, calculate the average side length DC ave Using the following formula, the average volume of the magnetic powder V ave (particle volume) is calculated. V ave =DC ave 3
[0104] (Cobalt ferrite particles) The cobalt ferrite particles preferably have uniaxial crystal anisotropy. The cobalt ferrite particles have uniaxial crystal anisotropy, which allows the magnetic powder to be preferentially crystal-oriented in the thickness direction (vertical direction) of the magnetic tape 22. The cobalt ferrite particles have, for example, a cubic shape. In this specification, the cubic shape includes a substantially cubic shape. The Co-containing spinel ferrite may further contain at least one of Ni, Mn, Al, Cu, and Zn in addition to Co.
[0105] The Co-containing spinel ferrite has, for example, an average composition represented by the following formula. Co x M y Fe 2 O Z (In the formula, M is at least one metal selected from the group consisting of Ni, Mn, Al, Cu, and Zn. x is a value within the range of 0.4≦x≦1.0. y is a value within the range of 0≦y≦0.3. However, x and y satisfy the relationship of (x+y)≦1.0. z is a value within the range of 3≦z≦4. A part of Fe may be substituted with another metal element.)
[0106] When the magnetic powder contains cobalt ferrite particles, the average particle size of the magnetic powder is 22 nm or less. The average particle size (average maximum particle size) of the magnetic powder is preferably 20 nm or less, more preferably 8 nm or more to 20 nm or less, even more preferably 10 nm or more to 18 nm or less, particularly preferably 10 nm or more to 16 nm or less, and most preferably 10 nm or more to 14 nm or less. When the average particle size of the magnetic powder is 22 nm or less, it is possible to obtain even better electromagnetic conversion characteristics (e.g., SNR) in a high recording density magnetic tape 22. On the other hand, when the average particle size of the magnetic powder is 8 nm or more, the dispersibility of the magnetic powder is further improved, and it is possible to obtain even better electromagnetic conversion characteristics (e.g., SNR). The method of calculating the average particle size of the magnetic powder is the same as the method of calculating the average particle size of the magnetic powder when the magnetic powder contains ε iron oxide particles.
[0107] The average aspect ratio of the magnetic powder is preferably 1.0 or more and 3.0 or less, more preferably 1.0 or more and 2.5 or less, even more preferably 1.0 or more and 2.1 or less, and particularly preferably 1.0 or more and 1.8 or less. When the average aspect ratio of the magnetic powder is within the range of 1.0 or more and 3.0 or less, aggregation of the magnetic powder can be suppressed. In addition, when the magnetic powder is vertically oriented in the process of forming the magnetic layer 43, the resistance applied to the magnetic powder can be suppressed. Therefore, the vertical orientation of the magnetic powder can be improved. The method of calculating the average aspect ratio of the magnetic powder is the same as the method of calculating the average aspect ratio of the magnetic powder when the magnetic powder contains ε iron oxide particles.
[0108] The average particle volume of the magnetic powder is preferably 5600 nm 3 Less than or equal to 250 nm, preferably 3 More than 4200nm 3 Less than or equal to 600 nm, and even more preferably 3 More than 3000nm 3 Below 600 nm, particularly preferably 3 More than 2200nm 3 Below 600 nm, most preferably 3 More than 1500nm 3 The average particle volume of the magnetic powder is 5600 nm or less. 3 If the average particle size of the magnetic powder is 25 nm or less, the same effect as when the average particle volume of the magnetic powder is 500 nm or less can be obtained. 3 When the average particle size of the magnetic powder is 8 nm or more, the same effect as that when the average particle size of the magnetic powder is 8 nm or more can be obtained. The method for calculating the average particle volume of the magnetic portion is the same as the method for calculating the average particle volume when the ε iron oxide particles have a cubic shape.
[0109] (Binding agent) Examples of the binder include thermoplastic resins, thermosetting resins, and reactive resins. Examples of the thermoplastic resins include vinyl chloride, vinyl acetate, vinyl chloride-vinyl acetate copolymers, vinyl chloride-vinylidene chloride copolymers, vinyl chloride-acrylonitrile copolymers, acrylic acid ester-acrylonitrile copolymers, acrylic acid ester-vinyl chloride-vinylidene chloride copolymers, acrylic acid ester-acrylonitrile copolymers, acrylic acid ester-vinylidene chloride copolymers, methacrylic acid ester-vinylidene chloride copolymers, methacrylic acid ester-vinyl chloride copolymers, methacrylic acid ester-ethylene copolymers, polyvinyl fluoride, vinylidene chloride-acrylonitrile copolymers, acrylonitrile-butadiene copolymers, polyamide resins, polyvinyl butyral, cellulose derivatives (cellulose acetate butyrate, cellulose diacetate, cellulose triacetate, cellulose propionate, nitrocellulose), styrene-butadiene copolymers, polyurethane resins, polyester resins, amino resins, and synthetic rubbers.
[0110] Examples of the thermosetting resin include phenol resin, epoxy resin, polyurethane curing resin, urea resin, melamine resin, alkyd resin, silicone resin, polyamine resin, and urea formaldehyde resin.
[0111] All of the above binders contain -SO 3 M, -OSO 3 M, -COOM, P=O(OM) 2 (wherein M represents a hydrogen atom or an alkali metal such as lithium, potassium, or sodium), -NR1R2, -NR1R2R3 + X - Side chain amines with terminal groups represented by >NR1R2 + X - (wherein R1, R2, and R3 each represent a hydrogen atom or a hydrocarbon group; X -represents a halogen element ion such as fluorine, chlorine, bromine, or iodine, an inorganic ion, or an organic ion.) Polar functional groups such as -OH, -SH, -CN, and an epoxy group may be introduced. The amount of these polar functional groups introduced into the binder is 10 -1 ~10 -8 mol / g, preferably 10 -2 ~10 -6 More preferably, it is expressed in moles / g.
[0112] (Lubricant) The lubricant contains at least one selected from, for example, fatty acids and fatty acid esters, preferably both fatty acids and fatty acid esters. The inclusion of a lubricant in the magnetic layer 43, particularly the inclusion of both a fatty acid and a fatty acid ester in the magnetic layer 43, contributes to improving the running stability of the magnetic tape 22. More particularly, the magnetic layer 43 contains a lubricant and has pores, thereby achieving good running stability. The improvement in running stability is believed to be due to the lubricant adjusting the dynamic friction coefficient of the magnetic layer 43 side surface of the magnetic tape 22 to a value suitable for running the magnetic tape 22.
[0113] The fatty acid may preferably be a compound represented by the following general formula (1) or (2). For example, the fatty acid may contain either a compound represented by the following general formula (1) or a compound represented by the following general formula (2), or may contain both.
[0114] The fatty acid ester may preferably be a compound represented by the following general formula (3) or (4). For example, the fatty acid ester may contain either a compound represented by the following general formula (3) or a compound represented by the following general formula (4), or may contain both.
[0115] By the lubricant containing either or both of a compound represented by general formula (1) and a compound represented by general formula (2), and either or both of a compound represented by general formula (3) and a compound represented by general formula (4), it is possible to suppress an increase in the dynamic friction coefficient of the magnetic tape 22 due to repeated recording or playback.
[0116] CH 3 (CH 2 ) k COOH (1) (However, in general formula (1), k is an integer selected from the range of 14 or more and 22 or less, more preferably from the range of 14 or more and 18 or less.)
[0117] CH 3 (CH 2 ) n CH=CH(CH 2 ) m COOH (2) (However, in general formula (2), the sum of n and m is an integer selected from the range of 12 to 20, more preferably from the range of 14 to 18.)
[0118] CH 3 (CH 2 ) p COO(CH 2 ) q CH 3 (3) (In the general formula (3), p is an integer selected from the range of 14 or more and 22 or less, more preferably from the range of 14 or more and 18 or less, and q is an integer selected from the range of 2 or more and 5 or less, more preferably from the range of 2 or more and 4 or less.)
[0119] CH 3 (CH 2 ) r COO-(CH 2 ) s CH(CH 3 ) 2 (4) (In the general formula (4), r is an integer selected from the range of 14 to 22, and s is an integer selected from the range of 1 to 3.)
[0120] (Antistatic agent) Examples of the antistatic agent include carbon black, natural surfactants, nonionic surfactants, and cationic surfactants.
[0121] (Abrasive) Examples of abrasives include acicular α-iron oxide obtained by dehydrating and annealing raw materials such as α-alumina with an α-conversion rate of 90% or more, β-alumina, γ-alumina, silicon carbide, chromium oxide, cerium oxide, α-iron oxide, corundum, silicon nitride, titanium carbide, titanium oxide, silicon dioxide, tin oxide, magnesium oxide, tungsten oxide, zirconium oxide, boron nitride, zinc oxide, calcium carbonate, calcium sulfate, barium sulfate, molybdenum disulfide, and magnetic iron oxide, and these may be surface-treated with aluminum and / or silica as necessary.
[0122] (hardening agent) Examples of the curing agent include polyisocyanates. Examples of the polyisocyanates include aromatic polyisocyanates such as an adduct of tolylene diisocyanate (TDI) and an active hydrogen compound, and aliphatic polyisocyanates such as an adduct of hexamethylene diisocyanate (HMDI) and an active hydrogen compound. The weight average molecular weight of these polyisocyanates is preferably in the range of 100 to 3000.
[0123] (rust inhibitor) Examples of the rust inhibitor include phenols, naphthols, quinones, heterocyclic compounds containing a nitrogen atom, heterocyclic compounds containing an oxygen atom, and heterocyclic compounds containing a sulfur atom.
[0124] (Non-magnetic reinforcing particles) Examples of non-magnetic reinforcing particles include aluminum oxide (α, β or γ alumina), chromium oxide, silicon oxide, diamond, garnet, emery, boron nitride, titanium carbide, silicon carbide, titanium carbide, titanium oxide (rutile or anatase type titanium oxide), and the like.
[0125] (base layer) The underlayer 42 serves to reduce the unevenness of the surface of the substrate 41 and adjust the unevenness of the surface of the magnetic layer 43. The underlayer 42 is a non-magnetic layer containing non-magnetic powder, a binder, and a lubricant. The underlayer 42 supplies the lubricant to the surface of the magnetic layer 43. The underlayer 42 may further contain at least one additive selected from the group consisting of an antistatic agent, a hardener, and an anti-rust agent, as necessary.
[0126] The average thickness of the underlayer 42 is preferably 0.3 μm or more and 2.0 μm or less, more preferably 0.5 μm or more and 1.4 μm or less. The average thickness of the underlayer 42 is determined in the same manner as the average thickness of the magnetic layer 43. However, the magnification of the TEM image is appropriately adjusted according to the thickness of the underlayer 42. When the average thickness of the underlayer 42 is 2.0 μm or less, the elasticity of the magnetic tape 22 due to an external force becomes even higher, making it even easier to adjust the width of the magnetic tape 22 by adjusting the tension.
[0127] (Non-magnetic powder) The non-magnetic powder includes at least one of inorganic particle powder and organic particle powder. The non-magnetic powder may also include carbon powder such as carbon black. One type of non-magnetic powder may be used alone, or two or more types of non-magnetic powder may be used in combination. The inorganic particles include, for example, metals, metal oxides, metal carbonates, metal sulfates, metal nitrides, metal carbides, or metal sulfides. The shape of the non-magnetic powder may be, for example, various shapes such as needle-like, spherical, cubic, and plate-like, but is not limited to these shapes.
[0128] (Binding agent, lubricant) The binder and lubricant are the same as those in the magnetic layer 43 described above.
[0129] (Additives) The antistatic agent, hardening agent and rust inhibitor are the same as those in the magnetic layer 43 described above.
[0130] (Back layer) The back layer 44 includes a binder and a non-magnetic powder. The back layer 44 may further include at least one additive selected from the group consisting of a lubricant, a hardener, and an antistatic agent, as necessary. The binder and the non-magnetic powder are the same as those of the underlayer 42 described above.
[0131] The average particle size of the non-magnetic powder is preferably 10 nm or more and 150 nm or less, more preferably 15 nm or more and 110 nm or less. The average particle size of the non-magnetic powder is determined in the same manner as the average particle size of the magnetic powder. The non-magnetic powder may contain non-magnetic powder having two or more particle size distributions.
[0132] The upper limit of the average thickness of the back layer 44 is preferably 0.6 μm or less. If the upper limit of the average thickness of the back layer 44 is 0.6 μm or less, the thickness of the underlayer 42 and the base material 41 can be kept thick even when the average thickness of the magnetic tape 22 is 5.6 μm or less, so that the running stability of the magnetic tape 22 in a recording and reproducing device can be maintained. The lower limit of the average thickness of the back layer 44 is not particularly limited, but is, for example, 0.2 μm or more.
[0133] The average thickness t of the back layer 44 b can be calculated as follows: First, the average thickness t T Measure the average thickness t T The method for measuring the thickness is as described in the "Average Thickness of Magnetic Tape" below. Next, the back layer 44 of the sample is removed with a solvent such as MEK (methyl ethyl ketone) or dilute hydrochloric acid. Next, the thickness of the sample is measured at five or more points using a Mitutoyo Laser Hologram (LGH-110C), and the measured values are simply averaged (arithmetic average) to obtain the average thickness t B Then, the average thickness t of the back layer 44 is calculated using the following formula: bThe measurement points are selected randomly from the sample. t b [μm]=t T [μm]-t B [μm]
[0134] The back layer 44 has a surface on which a large number of protrusions are provided. The large number of protrusions are intended to form a large number of holes in the surface of the magnetic layer 43 when the magnetic tape 22 is wound in a roll. The large number of holes are composed of, for example, a large number of non-magnetic particles protruding from the surface of the back layer 44.
[0135] (average thickness of magnetic tape) Average thickness (average total thickness) t of the magnetic tape 22 T The upper limit of the average thickness t of the magnetic tape 22 is 5.6 μm or less, preferably 5.0 μm or less, more preferably 4.6 μm or less, and even more preferably 4.4 μm or less. T When the average thickness t of the magnetic tape 22 is 5.6 μm or less, the recording capacity that can be recorded in one data cartridge can be increased compared to that of a general magnetic tape. T The lower limit of the thickness is not particularly limited, but is, for example, 3.5 μm or more. The total length of the magnetic tape 22 is 960 m or more.
[0136] The average thickness t of the magnetic tape 22 T is obtained as follows. First, a 1 / 2 inch wide magnetic tape 22 is prepared and cut into a length of 250 mm to prepare a sample. Next, a Mitutoyo Laser Hologram (LGH-110C) is used as a measuring device to measure the thickness of the sample at five or more points, and the measured values are simply averaged (arithmetic average) to obtain the average value t T The measurement points are selected randomly from the sample.
[0137] (Coercive force Hc) The upper limit of the coercive force Hc2 of the magnetic layer 43 in the longitudinal direction of the magnetic tape 22 is preferably 2000 Oe or less, more preferably 1900 Oe or less, and even more preferably 1800 Oe or less. If the coercive force Hc2 of the magnetic layer 43 in the longitudinal direction is 2000 Oe or less, sufficient electromagnetic conversion characteristics can be obtained even at high recording density.
[0138] The lower limit of the coercive force Hc2 of the magnetic layer 43 measured in the longitudinal direction of the magnetic tape 22 is preferably 1000 Oe or more. When the coercive force Hc2 of the magnetic layer 43 measured in the longitudinal direction is 1000 Oe or more, demagnetization due to leakage flux from the recording head can be suppressed.
[0139] The coercive force Hc2 is obtained as follows. First, three magnetic tapes 22 are stacked with double-sided tape, and then punched out with a φ6.39 mm punch to prepare a measurement sample. At this time, marking is performed with any non-magnetic ink so that the longitudinal direction (running direction) of the magnetic tape 22 can be recognized. Then, the MH loop of the measurement sample (whole magnetic tape 22) corresponding to the longitudinal direction (running direction) of the magnetic tape 22 is measured using a vibrating sample magnetometer (VSM). Next, the coating film (underlayer 42, magnetic layer 43, back layer 44, etc.) is wiped off using acetone or ethanol, etc., and only the substrate 41 remains. Then, three obtained substrates 41 are stacked with double-sided tape, and then punched out with a φ6.39 mm punch to prepare a sample for background correction (hereinafter simply referred to as "correction sample"). Thereafter, the MH loop of the calibration sample (substrate 41) corresponding to the perpendicular direction of the substrate 41 (perpendicular direction of the magnetic tape 22) is measured using the VSM.
[0140] The MH loop of the measurement sample (the entire magnetic tape 22) and the MH loop of the correction sample (substrate 41) are measured using a high-sensitivity vibration sample magnetometer "VSM-P7-15 type" manufactured by Toei Industry Co., Ltd. The measurement conditions are as follows: measurement mode: full loop, maximum magnetic field: 15 kOe, magnetic field step: 40 bits, time constant of locking amp: 0.3 sec, waiting time: 1 sec, number of MH averages: 20.
[0141] After the MH loop of the measurement sample (whole magnetic tape 22) and the MH loop of the correction sample (substrate 41) are obtained, the MH loop of the correction sample (substrate 41) is subtracted from the MH loop of the measurement sample (whole magnetic tape 22) to perform background correction and obtain the MH loop after background correction. The measurement and analysis program attached to the "VSM-P7-15" is used for this background correction calculation. The coercive force Hc2 is obtained from the obtained MH loop after background correction. The measurement and analysis program attached to the "VSM-P7-15" is used for this calculation. All of the above MH loop measurements are performed at 25°C. In addition, no "demagnetization field correction" is performed when measuring the MH loop in the longitudinal direction of the magnetic tape 22.
[0142] (Square ratio) The squareness ratio S1 of the magnetic layer 43 in the perpendicular direction (thickness direction) of the magnetic tape 22 is preferably 65% or more, more preferably 70% or more, even more preferably 75% or more, particularly preferably 80% or more, and most preferably 85% or more. When the squareness ratio S1 is 65% or more, the perpendicular orientation of the magnetic powder is sufficiently high, and therefore, even more excellent electromagnetic conversion characteristics (e.g., SNR) can be obtained.
[0143] The squareness ratio S1 in the vertical direction is obtained as follows. First, three magnetic tapes 22 are stacked with double-sided tape, and then punched with a φ6.39 mm punch to prepare a measurement sample. At this time, marking is performed with any non-magnetic ink so that the longitudinal direction (running direction) of the magnetic tape 22 can be recognized. Then, the MH loop of the measurement sample (whole magnetic tape 22) corresponding to the vertical direction (thickness direction) of the magnetic tape 22 is measured using a VSM. Next, the coating film (underlayer 42, magnetic layer 43, back layer 44, etc.) is wiped off using acetone or ethanol, etc., and only the substrate 41 remains. Then, three obtained substrates 41 are stacked with double-sided tape, and then punched with a φ6.39 mm punch to prepare a sample for background correction (hereinafter simply referred to as a "correction sample"). Then, the MH loop of the correction sample (substrate 41) corresponding to the vertical direction of the substrate 41 (vertical direction of the magnetic tape 22) is measured using a VSM.
[0144] The MH loop of the measurement sample (the entire magnetic tape 22) and the MH loop of the correction sample (substrate 41) are measured using a high-sensitivity vibration sample magnetometer "VSM-P7-15 type" manufactured by Toei Industry Co., Ltd. The measurement conditions are as follows: measurement mode: full loop, maximum magnetic field: 15 kOe, magnetic field step: 40 bits, time constant of locking amp: 0.3 sec, waiting time: 1 sec, number of MH averages: 20.
[0145] After the MH loop of the measurement sample (entire magnetic tape 22) and the MH loop of the correction sample (substrate 41) are obtained, background correction is performed by subtracting the MH loop of the correction sample (substrate 41) from the MH loop of the measurement sample (entire magnetic tape 22), and the MH loop after background correction is obtained. The measurement and analysis program attached to the "VSM-P7-15" is used for the calculation of this background correction.
[0146] The saturation magnetization Ms (emu) and residual magnetization Mr (emu) of the MH loop after background correction are substituted into the following formula to calculate the squareness ratio S1 (%). Note that all of the above MH loop measurements are performed at 25°C. Also, no "demagnetizing field correction" is performed when measuring the MH loop in the perpendicular direction to the magnetic tape 22. Note that this calculation uses the measurement and analysis program provided with the "VSM-P7-15 model." do. Squareness ratio S1(%)=(Mr / Ms)×100
[0147] The squareness ratio S2 of the magnetic layer 43 in the longitudinal direction (running direction) of the magnetic tape 22 is preferably 35% or less, more preferably 30% or less, even more preferably 25% or less, particularly preferably 20% or less, and most preferably 15% or less. When the squareness ratio S2 is 35% or less, the magnetic powder has a sufficiently high vertical orientation, so that even better electromagnetic conversion characteristics (e.g., SNR) can be obtained.
[0148] The squareness ratio S2 in the longitudinal direction is determined in the same manner as the squareness ratio S1, except that the MH loop is measured in the longitudinal direction (running direction) of the magnetic tape 22 and the substrate 41.
[0149] (Back surface roughness Rb) Surface roughness of the back surface (surface roughness of the back layer 44) R b But R b The surface roughness R of the back surface is preferably ≦6.0 [nm]. b When it is in the above range, even better electromagnetic conversion characteristics can be obtained.
[0150] [Variations] In the above embodiment, a tape reel for a tape cartridge that complies with the LTO standard has been used as an example, but the present technology can also be applied to tape reels for tape cartridges that comply with standards other than LTO and tape cartridges equipped with such tape reels.
[0151] The present technology can also be configured as follows. (1) a first flange; A second flange; a cylindrical reel hub having a first end portion integrally formed with the first flange, a second end portion to which the second flange is joined, and an outer circumferential surface on which a magnetic tape is wound; Equipped with The outer circumferential surface of the reel hub is a first outer circumferential region that expands in diameter from the first end toward the second end; a second outer circumferential region that expands in diameter from the first outer circumferential region to the second end and forms a ridge portion that is convex toward the radially outward side of the reel hub on the boundary with the first outer circumferential region; Tape reel. (2) The tape reel according to (1) above, The ridge portion is located closer to the first end portion than the center of the height of the reel hub. Tape reel. (3) The tape reel according to (1) or (2) above, a difference between an outer diameter of the ridge portion and an outer diameter of the first end portion is 10 μm or more and 50 μm or less; The difference between the outer diameter of the first end portion and the outer diameter of the second end portion is 30 μm or more and 90 μm or less. Tape reel. (4) The tape reel according to (3) above, The first flange and the reel hub are molded bodies made of a composite material containing a synthetic resin material and a glass filler. Tape reel. (5) The tape reel according to (4) above, The synthetic resin material is a polycarbonate resin, and the content of the glass filler is 10% or more and 20% or less by weight relative to the polycarbonate resin. Tape reel. (6) The tape reel according to any one of (1) to (5) above, The height of the reel hub is approximately 13 mm. The length from the first end to the ridge is 3 mm or more and 5 mm or less. Tape reel. (7) A tape reel having a first flange, a second flange, and a cylindrical reel hub having a first end connected to the first flange, a second end connected to the second flange, and an outer circumferential surface around which a magnetic tape is wound. Equipped with The outer circumferential surface of the reel hub is a first outer circumferential region that expands in diameter from the first end toward the second end; a second outer circumferential region that expands in diameter from the first outer circumferential region to the second end and forms a ridge portion that is convex toward the radially outward side of the reel hub on the boundary with the first outer circumferential region; Tape cartridge. (8) The tape cartridge according to (7) above, After storing the tape cartridge for one week in an environment with a temperature of 49° C. and a relative humidity of 80% with the magnetic tape wound on the tape reel, the difference in radius between the first end and the second end is 10 μm or less. Tape cartridge. (9) The tape reel according to (7) or (8) above, The magnetic tape has a thickness of 5.6 μm or less and a length of 960 m or more. Tape cartridge. (10) A manufacturing apparatus for a tape reel including the reel hub described in (1) above, A first die for forming an outer peripheral surface of the reel hub; a second die for forming the inner peripheral surface of the reel hub; Equipped with The first mold comprises: a first molding surface formed of a tapered surface that forms the first outer circumferential region; and a second molding surface formed of a cylindrical surface that forms the second outer circumferential region. Tape reel manufacturing equipment. [Explanation of symbols]
[0152] 1...Tape cartridge 5...Tape reel 6…Reel hub 6a...Lower end 6b...Top end 6d...Outer surface 6d1…First outer region 6d2…Second outer perimeter 6d3…Ridge 7…Bottom flange 8...Upper flange 22...Magnetic tape
Claims
1. A first flange; A second flange; a cylindrical reel hub having a first end portion integrally formed with the first flange, a second end portion to which the second flange is joined, and an outer circumferential surface on which a magnetic tape is wound; Equipped with The outer circumferential surface of the reel hub is a first outer circumferential region that expands in diameter from the first end toward the second end; a second outer circumferential region that expands in diameter from the first outer circumferential region to the second end and forms a ridge portion that is convex radially outward of the reel hub on a boundary with the first outer circumferential region, The ridge portion is located closer to the first end portion than the center of the height of the reel hub. Tape reel.
2. 2. The tape reel of claim 1, a difference between an outer diameter of the ridge portion and an outer diameter of the first end portion is 10 μm or more and 50 μm or less; The difference between the outer diameter of the first end portion and the outer diameter of the second end portion is 30 μm or more and 90 μm or less. Tape reel.
3. 3. The tape reel of claim 2, The first flange and the reel hub are molded bodies made of a composite material containing a synthetic resin material and a glass filler. Tape reel.
4. 4. The tape reel of claim 3, The synthetic resin material is a polycarbonate resin, and the content of the glass filler is 10% or more and 20% or less by weight relative to the polycarbonate resin. Tape reel.
5. 2. The tape reel of claim 1, The height of the reel hub is approximately 13 mm. The length from the first end to the ridge line is 3 mm or more and 5 mm or less. Tape reel.
6. A tape reel comprising: a first flange; a second flange; and a cylindrical reel hub having a first end connected to the first flange, a second end connected to the second flange, and an outer circumferential surface around which a magnetic tape is wound. Equipped with The outer circumferential surface of the reel hub is a first outer circumferential region that expands in diameter from the first end toward the second end; a second outer circumferential region that expands in diameter from the first outer circumferential region to the second end and forms a ridge portion that is convex radially outward of the reel hub on a boundary with the first outer circumferential region, The ridge portion is located closer to the first end portion than the center of the height of the reel hub. Tape cartridge.
7. 7. The tape cartridge of claim 6, After storing the tape cartridge for one week in an environment having a temperature of 49° C. and a relative humidity of 80% with the magnetic tape wound around the tape reel, the difference in radius between the first end and the second end is 10 μm or less. Tape cartridge.
8. 7. The tape cartridge of claim 6, The magnetic tape has a thickness of 5.6 μm or less and a length of 960 m or more. Tape cartridge.
Citation Information
Patent Citations
Reel and recording tape cartridge
JP2007066466A
Tape reel, recording tape cartridge, machine reel, and drive unit
JP2008243294A
Tape reel, recording tape cartridge, machine reel, lead member, and drive apparatus
JP2008276868A
Reel and recording tape cartridge
JP2009048692A
Tape reel and tape cartridge
WO2020202980A1