Optical film, polarizing plate, and image display device

The optical film with a spectral transmittance adjuster and laminated structure effectively blocks blue light without yellowing and maintains thinness, addressing issues of yellow tint and adhesive strength in existing films.

JP7571832B2Active Publication Date: 2024-10-23DAI NIPPON PRINTING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023128940
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-01-31
Filing Date
2023-08-08
Publication Date
2024-10-23
Estimated Expiration
2038-01-30

AI Technical Summary

Technical Problem

Existing optical films fail to effectively block blue light without causing yellow tint and require thick adhesive layers, leading to potential peeling issues.

Method used

Incorporating a spectral transmittance adjuster into a thin light-transmitting functional layer that allows blue light to be blocked while allowing light in the 410 nm to 440 nm range to pass, with a thickness of 9 μm or less, and using a laminated structure to enhance performance.

Benefits of technology

The solution effectively blocks blue light, prevents yellowing, and maintains thinness, ensuring high transparency and adhesive strength, suitable for use in image display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571832000024
    Figure 0007571832000024
  • Figure 0007571832000025
    Figure 0007571832000025
  • Figure 0007571832000026
    Figure 0007571832000026
Patent Text Reader

Abstract

To provide an optical film that can block blue light, can suppress yellowish coloring, and can be made thin, a polarizer with such an optical film, and an image display unit.SOLUTION: There is provided an optical film 10 that comprises a light-transmissive base material 11 and a light-transmitting function layer 12 provided on one surface side of the light-transmissive base material 11, and also has a spectral transmission factor of less than 1% at a wavelength of 380 nm, equal to or greater than 10% and less than 60% at 410 nm, and equal to or greater than 70% at 440 nm, and the light-transmitting function layer 12 is 9 μm or smaller thick.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

REFERENCE TO RELATED APPLICATIONS

[0001] This application is a continuation of the prior Japanese application No. 2017-15454 (filing date: January 2017) No. 6,313,635, filed on Dec. 31, 2003, the entire disclosure of which is incorporated herein by reference. and is incorporated herein by reference. [Technical field]

[0002] The present invention relates to an optical film, a polarizing plate, and an image display device. [Background technology]

[0003] In recent years, LEDs have been used as backlight sources for image display devices such as personal computers and tablets. LEDs (Light Emitting Diodes) are being actively adopted for this purpose, This LED emits a strong light called blue light.

[0004] Blue light has a wavelength of 380 to 495 nm and is strong, with properties similar to ultraviolet light. Because it has energy, it reaches the retina without being absorbed by the cornea or lens, and It is said that this can cause damage to the eyes, eye fatigue, and adverse effects on sleep. It is desirable to block blue light in devices.

[0005] As a method for solving such a problem of blue light, for example, The optical film is made of a light-transmitting substrate and a light-transmitting functional layer, and a dye and a UV-absorbing agent are added to the substrate and the light-transmitting functional layer. One possible method is to incorporate an agent into the composition (see, for example, JP 2014-10947 A).

[0006] In addition, the display panel is protected from external ultraviolet light and some visible light by blocking it. In order to achieve this, a dye and / or an ultraviolet absorbing agent is added to the adhesive layer constituting the optical film. Methods for doing so are also being considered. Summary of the Invention [Problem to be solved by the invention]

[0007] However, the dyes and / Or the ultraviolet absorber has a relatively short absorption wavelength range centered around 300 to 360 nm. Since the wavelengths were in a narrow range, the blue light blocking performance was not sufficient.

[0008] On the other hand, the relatively long wavelength region of blue light affects the color of transmitted light. Therefore, if the light absorbs too much in the relatively long wavelength region, the optical film will take on a yellowish tint. There is a saying.

[0009] Furthermore, when the adhesive layer contains a dye and / or an ultraviolet absorbing agent, the adhesive strength is low. This may result in peeling or floating off from the substrate during environmental testing. For this reason, the thickness of the adhesive layer needs to be 10 μm or more, which makes it necessary to make the optical film thinner. It may not be possible to measure this.

[0010] In view of the above-mentioned current situation, the present invention provides a thin type liquid crystal display that can block blue light and suppress yellowish color. Optical film capable of improving image quality, polarizing plate and image forming method using the same, The object is to provide a display device. [Means for solving the problem]

[0011] The present inventors have conducted extensive research into the above-mentioned problem, and have found that the wavelength of blue light While it sufficiently absorbs light in the wavelength range of 380 nm or less, it also absorbs light in the wavelength range of around 410 nm. To transmit light in the wavelength range moderately and to transmit light with a wavelength of 440 nm or more sufficiently This makes it possible to block blue light and suppress the yellowish tint of the optical film. The transmittance adjusting agent is incorporated into the thin light-transmitting functional layer instead of the adhesive layer, resulting in a thinner film. The present invention has been completed based on the findings.

[0012] According to one aspect of the present invention, there is provided a light-transmitting substrate and a light-transmitting layer provided on one surface side of the light-transmitting substrate. and a light-transmitting functional layer having a spectral transmittance at a wavelength of 380 nm. The spectral transmittance at a wavelength of 410 nm is 10% or more and less than 60%. and the spectral transmittance at a wavelength of 440 nm is 70% or more, An optical film is provided having a thickness of 9 μm or less.

[0013] The optical film has a yellow index of 1 or more and 12 or less. It may be the following.

[0014] In the above optical film, the blue light blocking rate of the optical film is 30% or more. may be also possible.

[0015] In the above optical film, the wavelength of 410 nm to 420 nm obtained by using the least squares method The slope of the transmission spectrum in this range may be 2 or more.

[0016] In the above optical film, the arithmetic average roughness (Ra) of the surface of the optical film is 10n It may be less than m.

[0017] The optical film may have an uneven surface.

[0018] In the above optical film, the light-transmitting functional layer contains a resin and a spectral transmittance adjusting agent. The optical filter may further include a spectral transmittance adjusting layer.

[0019] In the optical film, the light-transmitting functional layer includes a spectral transmittance adjusting layer and a spectral transmittance adjusting layer. and an overcoat layer provided on the opposite side of the transmittance adjusting layer to the light-transmitting substrate side. It is also possible to do so.

[0020] In the optical film, the light-transmitting functional layer includes a spectral transmittance adjusting layer and a spectral transmittance adjusting layer. A plurality of vapor-deposited layers having a laminated structure provided on the side of the transmittance adjusting layer opposite to the light-transmitting substrate side. The device may also include:

[0021] In the optical film, the light-transmitting functional layer includes a spectral transmittance adjusting layer and a spectral transmittance adjusting layer. The reflectance adjusting layer is provided on the surface opposite to the surface on the light-transmitting substrate side, and the reflectance adjusting layer is refracted by the reflectance adjusting layer. The optical fiber 10 may have a plurality of invisible layers having a laminated structure with different optical fiber ratios.

[0022] In the optical film, the light-transmitting functional layer includes a spectral transmittance adjusting layer and a spectral transmittance adjusting layer. A transmittance adjusting layer is provided on the side opposite to the light-transmitting substrate, and the refractive index is the same as that of the spectral transmittance layer. The optical element may further include a low refractive index layer having a refractive index lower than that of the optical element.

[0023] According to another aspect of the present invention, there is provided the optical film, and a film provided on one side of the optical film. and a polarizer disposed adjacent the polarizer.

[0024] According to another aspect of the present invention, there is provided a display element, and a display device disposed on the viewer side of the display element. There is provided an image display device comprising the optical film or the polarizing plate.

[0025] In the above image display device, the display element may be an organic light-emitting diode display element. good. Effect of the Invention

[0026] According to one aspect of the present invention, it is possible to block blue light, suppress yellowish color, and reduce thickness. According to another aspect of the present invention, there is provided an optical film capable of achieving the above object. If such an optical film is used, it is possible to provide a polarizing plate and an image display device equipped with such an optical film. do. [Brief description of the drawings]

[0027] [Figure 1] FIG. 1 is a schematic diagram of an optical film according to an embodiment. [Diagram 2] FIG. 2 is a graph showing an example of the spectral transmittance of the optical film according to the embodiment. [Diagram 3] FIG. 3 is a schematic diagram of another optical film according to an embodiment. [Figure 4] FIG. 4 is an explanatory diagram of a method for measuring θa. [Diagram 5] FIG. 5 is a schematic diagram of another optical film according to an embodiment. [Figure 6] FIG. 6 is a schematic diagram of another optical film according to an embodiment. [Figure 7] FIG. 7 is a schematic diagram of another optical film according to an embodiment. [Figure 8] FIG. 8 is a schematic diagram of a polarizing plate according to an embodiment. [Figure 9] FIG. 9 is a schematic configuration diagram of an image display device according to an embodiment. [Figure 10] FIG. 10 is a graph showing the spectral transmittance of the optical films according to the examples and the comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Hereinafter, the optical film and the image display device according to the embodiments of the present invention will be described with reference to the drawings. In this specification, the terms "film" and "sheet" are used interchangeably. Thus, for example, "film The term "sheet" is used to include members such as sheets. FIG. 2 is a schematic diagram of an optical film according to the present embodiment, and shows an example of the spectral transmittance of the optical film. 3 and 5 to 7 are graphs showing schematic configurations of other optical films according to this embodiment. FIG. 4 is an explanatory diagram of a method for measuring θa.

[0029] <<<<Optical films>>>> The optical film 10 shown in FIG. 1 has a spectral transmittance of less than 1% at a wavelength of 380 nm. The spectral transmittance at a wavelength of 410 nm is between 10% and 60%. The spectral transmittance at a wavelength of 440 nm is 70% or more. If the spectral transmittance at a wavelength of 380 nm is 1% or more, the blocking rate of blue light is reduced. Therefore, the problem of blue light may not be solved. If the spectral transmittance at a wavelength of 410 nm is less than 10%, the yellowish tint of the optical film is suppressed. In addition, the spectral transmittance at a wavelength of 410 nm is 60% or more. However, the problem of blue light cannot be solved, and transmitted light may have a negative effect. If the spectral transmittance at a wavelength of 440 nm is less than 70%, the yellow index The optical film itself has a yellowish color and the transmittance in the visible light region is reduced. Therefore, the properties may not be suitable for optical films.

[0030] The spectral transmittance was measured by cutting an optical film into a size of 50 mm x 50 mm and setting the transmittance to 0 A spectrophotometer capable of measuring in 0.5% increments (product name: UV-2450, Shimadzu Corporation) The light-transmitting substrate side of the optical film is placed in the light source (tungsten lamp and deuterium lamp). The wavelengths were 380 nm and 410 nm under the following measurement conditions. Measure the transmittance at least 5 points within 1 nm at 440 nm and 440 nm. The average value is calculated by measuring the wavelengths of 380 nm and 41 The spectral transmittance at 0 nm and 440 nm was calculated by measuring three times. If there are any undulations in the spectrum of the spectral transmittance, use Delta 5 Smoothing processing may be performed at .0 nm. (Measurement conditions) ·Wavelength range: 300nm~780nm Scan speed: Fast Slit width: 2.0 Sampling interval: Auto (0.5 nm interval) ·Lighting:C Light source: D2 and WI ·Field of view: 2° Light source switching wavelength: 360nm S / R Switching: Standard Detector: PM Autozero: Performed at 550 nm after baseline scan

[0031] The optical transmittance of the optical film 10 is almost 0% up to a wavelength of 380 nm. The light transmission gradually increases from 0 nm, and the light transmission increases suddenly at a wavelength of around 440 nm. Specifically, for example, as shown in FIG. At 0, the spectral transmittance curve forms a sigmoid shape between 380 nm and 440 nm. It has changed like this.

[0032] In the optical film 10, in order to more effectively block blue light, The spectral transmittance at is preferably less than 0.5%, more preferably less than 0.2%. In the optical film 10, from the viewpoint of further suppressing yellowish color, it is more preferable to use The lower limit of the spectral transmittance at nm is preferably more than 10%, and is preferably 13% or more. More preferably, the ratio is 15% or more. From the perspective of blue light blocking performance, the upper limit of the spectral transmittance at a wavelength of 410 nm is The optical film is preferably less than 58%, and more preferably 55% or less. In the case of 10, the spectral transmittance at a wavelength of 440 nm is suppressed from decreasing visibility due to coloring and From the viewpoint of ensuring transparency, it is preferable that the ratio is 75% or more, and 80% or more. is more preferred.

[0033] The optical film 10 has a spectral transmittance of 45% or more and 70% or less at a wavelength of 420 nm. It is preferable that the spectral transmittance at a wavelength of 420 nm is within this range. , demonstrate blue light blocking performance, suppress the decrease in visibility due to coloring, and ensure transparency. The spectral transmittance of the optical film 10 at a wavelength of 420 nm is also It shall be measured in the same manner as the spectral transmittance at 80 nm, etc.

[0034] In the optical film 10, the spectral transmittance in the wavelength range of 480 nm to 780 nm is The maximum spectral transmittance in the range of 400 to 450 nm is not decreased by more than 10%. In order to reduce the yellow index described later, the spectral transmittance adjusting layer is preferably It is also possible to add dyes with different absorption wavelength ranges that absorb light from 480 to 780 nm. However, when a dye with a different absorption wavelength range is added, the spectral transmittance in the wavelength range of 480nm to 780nm In contrast, in the optical film 10, A low yellow ink is obtained without adding a dye having a different absorption wavelength range to the spectral transmittance adjusting layer 13 described later. The spectral transmittance is calculated by cutting the sample into a size of 50 mm x 50 mm. The optical film was then measured using a spectrophotometer (product name: UV- 2450, Shimadzu Corporation, light source: tungsten lamp and deuterium lamp) The optical film is placed in the container so that the light-transmitting substrate side faces the light source. For 0 nm, the transmittance for at least 5 points within 1 nm before and after each wavelength is 480 For the wavelength range from 780 nm to 790 nm, the transmittance noise caused by the film interference was corrected. For each wavelength, the transmittance of all points detected within 20 nm was measured. The average value of the measured values ​​is calculated. The measurement conditions for the spectral transmittance are as follows: The measurement conditions for the spectral transmittance at the wavelengths of 380 nm, 410 nm, and 440 nm are as follows: Same here.

[0035] When other films such as polarizing plates are attached to the optical film via a pressure-sensitive adhesive layer or bonding layer The adhesive layer and other films are peeled off, and then the wavelengths are 380 nm and 410 nm. The spectral transmittance at 420 nm, 420 nm, and 440 nm shall be measured. The peeling can be performed, for example, as follows. First, a pressure-sensitive adhesive layer or a bonding layer is applied to the optical film. The laminate with the other film attached through the adhesive layer is heated with a dryer to separate the optical film from the other film. Insert the tip of the cutter into the area that seems to be the film interface and slowly peel it off. By repeating this heating and peeling process, the adhesive layer, the bonding layer and other films can be peeled off. Even if such a peeling process is performed, it does not have a significant effect on the measurement of the spectral transmittance. There is no sound.

[0036] The optical film 10 preferably has a yellow index (YI) of 1 or more and 12 or less. If the YI of the optical film is less than 1, the blue light blocking rate decreases. In addition, if the YI of the optical film exceeds 12, the yellowish tinge of the optical film becomes noticeable. In other words, it may not be applicable to applications where transparency is required. ) is a spectrophotometer (product name " UV-2450, manufactured by Shimadzu Corporation, light source: tungsten lamp and deuterium lamp The light was measured with the optical film placed in the hood so that the light-transmitting substrate side was facing the light source. From the transmittance of optical films at wavelengths of 300 nm to 780 nm, JIS Z8722:2009 Calculate the chromaticity tristimulus values ​​X, Y, and Z according to the formula given in This value is calculated according to the formula described in ASTM D1925:1962. Low index (YI) is the wavelength of 300nm to 780nm for one optical film. The transmittance was measured three times and calculated three times, and the arithmetic mean value of the three calculated values ​​was calculated. In addition, in the case of UV-2450, the yellow index is the value obtained by contacting UV-2450. On the connected monitor, read the transmittance measurement data and enter the "YI" item in the calculation items. The transmittance of the light from 300nm to 780nm is calculated by checking the box. The measurement conditions were: spectral transmittance at wavelengths of 380 nm, 410 nm, and 440 nm The measurement conditions are the same as those for the YI. The lower limit of the YI is preferably low from the viewpoint of ensuring high transparency. However, if you want to add blue light blocking performance, it is recommended to use 2 or more, 3 or more. However, if YI is too large, the color will turn yellow. For this reason, the upper limit of YI is 10 or less, 7 or less, and 6 or less. It is more preferable that it is lower (smaller numbers are better).

[0037] In addition, other films such as a polarizing plate are provided on the optical film via an adhesive layer or a bonding layer. If the adhesive layer is not attached, peel off the other film together with the adhesive layer in the same manner as above. The yellow index (YI) is measured from the above. Even if there was, it would not have a significant effect on the Yellow Index (YI) measurement.

[0038] The optical film 10 preferably has a blue light blocking rate of 30% or more. If the blue light blocking rate is less than 30%, the problems caused by blue light mentioned above will not be fully resolved. Such a blue light blocking rate may not be able to be solved by, for example, a spectral transmittance adjusting layer. By including a sesamol-type benzotriazole monomer as described below in 13, the following can be achieved. The above blue light blocking rate is calculated according to JIS T7333:2005. The value is calculated as follows. First, cut it into a size of 50 mm x 50 mm. The optical film was measured using a spectrophotometer (product name: UV -2450, manufactured by Shimadzu Corporation, light source: tungsten lamp and deuterium lamp) The optical film is placed in the room so that the substrate side faces the light source. At 5 nm, the transmittance is measured at least 5 points between 1 nm before and after, and the average By calculating the values, the spectral transmittances of wavelengths from 380 nm to 495 nm are determined. The blue light blocking rate (%) is A, and the average transmittance from 380 nm to 495 nm is B. The value (%) is B, and the blue light blocking rate is calculated using the following formula. The coverage is the arithmetic average of three measurements. The measurement conditions for the spectral transmittance are as follows: The same conditions for measuring the spectral transmittance at wavelengths of 380 nm, 410 nm, and 440 nm were used as above. It seems that. A=100-B

[0039] In addition, other films such as a polarizing plate are provided on the optical film via an adhesive layer or a bonding layer. If the adhesive layer is not attached, peel off the other film together with the adhesive layer in the same manner as above. The blue light blocking rate is measured from the above. However, this does not have a significant impact on the measurement of blue light blocking rate.

[0040] The optical film 10 has a wavelength range of 410 nm to 420 nm obtained by using the least squares method. It is preferable that the slope of the transmission spectrum is 2 or more. If the slope is 2 or more, It is rich in light wavelengths in the blue light range, for example, wavelengths in the range of 380 nm to 495 nm. It can cut light in small amounts. It also blocks blue light in the wavelength range (380nm to 495nm). If too much light is cut, the backlight of the image display device or the emission wavelength region (e.g., O This interferes with the LED's 430 nm wavelength light, resulting in poor color reproduction, especially with YI. However, if the above slope is 2 or more, The above-mentioned inclination is to selectively cut off the light of the target wavelength. From the viewpoint of the transmission efficiency, the larger the gradient, the more preferable. Therefore, the upper limit of the gradient is not particularly limited. The upper limit of the slope can be, for example, 20 or less, or 10 or less.

[0041] The above inclination is calculated as follows. First, the size is 50 mm x 50 mm. The optical film cut into pieces is then measured using a spectrophotometer capable of measuring the transmittance in 0.5% increments, for example. (Product name: UV-2450, manufactured by Shimadzu Corporation) The substrate side of the optical film is the light source. When the laser was placed so that the laser was on the side of the target, the laser was placed at 1 nm forward and backward at wavelengths of 410 nm to 420 nm. The transmittance is measured at a minimum of five points over a distance of 4 m, and the average value is calculated. The spectral transmittance from 10 nm to 420 nm is then measured. Then, the slope of the spectral transmittance at wavelengths of 410 nm to 420 nm is calculated by the least squares method. The above slope is the arithmetic average value obtained by measuring three times. The conditions were as follows: measurement of the spectral transmittance at the wavelengths of 380 nm, 410 nm, and 440 nm. The conditions are the same.

[0042] The optical film 10 preferably has antistatic properties. The optical film 10 has a light-preventing property, and is therefore particularly suitable for use in IPS liquid crystal display devices. In addition, when the liquid crystal display device is an IPS type liquid crystal display device, an optical filter can be used. The surface resistance of film 10 is 10 10 It is preferable that the resistance is 10Ω / □ or less. 9 Ω / □ or less In particular, the liquid crystal display device is an IPS type with an in-cell touch panel. In the case of a liquid crystal display device, the surface resistance of the optical film 10 is 10 7 Ω / □ or more 10 1 0 It is preferable that the liquid crystal display device is an IPS type with an in-cell touch panel. In the case of a liquid crystal display device of the type, the lower limit of the surface resistance value of the optical film 10 is 10 8 Ω / □ More preferably, the upper limit is 10 9 It is more preferable that the resistance is Ω / □ or less.

[0043] The surface resistance was measured using a resistivity meter (product name: Hirester UP MCP-HT450, manufactured by Mitsubishi Chemical Analytech Co., Ltd. (Probe: URS probe (MCP-HTP14)) The measurements were taken at an applied voltage of 500 V under an environment of 25±4°C and 50±10% humidity. This shall be the case.

[0044] The antistatic performance is achieved by adding an antistatic agent to the light-transmitting functional layer 12 constituting the optical film 10. The antistatic agent is not particularly limited, and may be any of the conventionally known antistatic agents. For example, cationic antistatic agents such as quaternary ammonium salts, , tin-doped indium oxide (ITO), antimony-doped tin oxide (ATO), etc. When the above antistatic agent is used, its content is It is preferably from 1% by mass to 30% by mass based on the total mass of all solid contents.

[0045] The optical film 10 is preferably foldable. Light transmission function according to the mandrel test described in K5600-5-1:1999 The optical film 10 is wound around a stainless steel rod having a diameter of 2 mm so that the layer 12 is on the outside or inside. It is preferable that no cracks occur in the optical film 10 when the optical film 10 is attached. The Drell test involves cutting an optical film into a size of 100 mm x 25 mm and then Wrap the optical film around the stainless steel rod so that both ends of the long side of the film face each other, and hold for 5 seconds. After that, the optical film was released, and the optical film that was in contact with the stainless steel rod was removed. Check whether cracks have occurred along the short side of the film.

[0046] Another film such as a polarizing plate is provided on one side of the optical film 10 via an adhesive layer or bonding layer. If the adhesive layer is attached to the film, remove it together with the adhesive layer and other films in the same manner as above. The mandrel test shall be carried out after peeling off the wire. Even so, this does not have a significant effect on the results of the mandrel test.

[0047] The optical film 10 includes a light-transmitting substrate 11 and a light-transmitting layer 12 provided on one side of the light-transmitting substrate 11. The term "light-transmitting functional layer" as used herein means a light-transmitting functional layer 12. It has optical transparency and is intended to perform some function in an optical film. Specifically, the light-transmitting functional layer is, for example, a spectral transmittance adjusting layer, an overcoat layer, Examples of the layer include an anti-glare layer, an invisible layer, a refractive index adjusting layer, an anti-fouling layer, or a combination thereof. The light-transmitting functional layer may have a single-layer structure, but may have two or more light-transmitting functional layers stacked together. It may have a multi-layer structure.

[0048] The surface 10A of the optical film 10 is the surface 12A of the light-transmitting functional layer 12. The "surface of the light-transmitting functional layer" refers to the surface of the light-transmitting functional layer opposite to the surface of the light-transmitting substrate. This means the surface.

[0049] The arithmetic mean roughness R of the surface 10A of the optical film 10 (the surface 12A of the light-transmitting functional layer 12) It is preferable that a is less than 10 nm. When the above Ra is satisfied, the optical film 10 has It is a clear film with extremely excellent transparency. The above Ra is 50 mm The surface of the optical film was cut to a size of ×50 mm and measured with a surface roughness measuring instrument (product name Using the "SE-3400" manufactured by Kosaka Laboratory Co., Ltd., under the following measurement conditions, JIS B0 It can be determined by measuring in accordance with the method in accordance with 601:1994. (1) Stylus for detecting surface roughness (Kosaka Laboratory product name "SE2555N" (2μm standard) ) Tip curvature radius 2μm, apex angle 90 degrees, material diamond (2) Measurement conditions of surface roughness measuring instrument - Reference length (cutoff value λc of roughness curve): 0.8 mm Evaluation length (reference length (cutoff value λc) x 5): 4.0 mm Stylus feed speed: 0.5mm / s Reserve length: (Cutoff value λc) x 2 Longitudinal magnification: 20,000x ·Horizontal magnification: 10x

[0050] The Ra is the value at which there is no abnormality, at least when visually observed, on the surface 10A of the optical film 10. Three areas without any large foreign objects or scratches were randomly selected and The upper limit of Ra is 8 nm or less. This is more preferable.

[0051] The above Ra was measured using an atomic force microscope (product name "WET-9100", manufactured by Shimadzu Corporation). It is also possible to measure it using a 50mm x 50mm cut. On the surface of the optical film, there are at least some areas of the optical film that are visually normal. Three locations (locations without large foreign objects or scratches) were randomly selected and cut into 5 mm squares. On the other hand, a flat circular sample with a diameter of 15 mm and a thickness of 1 mm was obtained. Prepare several metal plates and attach a carbon double-sided tape manufactured by Nissin EM Co., Ltd. to each metal plate. Affix one sample on the tape, so that the sample surface (optical film surface) Then, to ensure that the tape and the sample are firmly attached, To measure the temperature, the metal plate with the sample is left in a desiccator overnight. The metal plate was placed on the measurement stage of an atomic force microscope (product name "WET-9400", manufactured by Shimadzu Corporation). The sample was fixed to the sample with a magnet, and the measurement area was 5 μm square in tapping mode, and the sample was measured with an atomic force microscope. The surface shape is observed. The surface analysis software built into the atomic force microscope calculates the surface shape from the observed data. The Ra is calculated using surface analysis software. Note that the vertical scale for surface analysis is 20 nm. The observation was performed at room temperature, and the cantilever was a NanoWorld NCHR-2 0 is used. In addition, five points are randomly selected for each sample for observation. Then, observe the surface shape of each of the 3 samples x 5 locations (total of 15 points). For all 15 data points obtained, the surface analysis software built into the atomic force microscope was used to perform R Calculate a and the arithmetic mean value of the 15 points is the Ra of the sample.

[0052] The use of the optical film 10 is not particularly limited, but examples of the use of the optical film 10 include: For example, smartphones, tablet devices, personal computers (PCs), wearables Image display devices such as mobile terminals, digital signage, televisions, and car navigation systems The optical film 10 is also suitable for use in vehicles. The form of the product is that it is used in applications that require flexibility, such as foldable and rollable. Also preferred.

[0053] The optical film 10 may be cut to a desired size, or may be in a roll. When the optical film 10 is cut to a desired size, the size of the optical film is not particularly limited and is appropriately determined depending on the size of the display surface of the image display device. The size of the optical film 10 is, for example, 2.8 inches or more and 500 inches or less. In this specification, "inch" means that when the optical film has a rectangular shape, It means the length of the diagonal, in the case of a circle, it means the diameter, in the case of an ellipse, The average value of the sum of the minor axis and the major axis is used here. In this case, the aspect ratio of the optical film when calculating the above inches is the display screen of the image display device. There is no particular limitation as long as there is no problem. For example, vertical:horizontal=1:1, 4:3, 16:10, 16 However, especially for in-vehicle applications and digital signage, The aspect ratio of the optical film 10 is not limited to this. If the size is large, cut it out from any position to A5 size (148mm x 210mm). Then, cut out to the size of each measurement item.

[0054] <<<Light transparent base material>>> The light-transmitting substrate 11 is a substrate having light transmittance. The resin is not particularly limited, and examples thereof include polyester resins and acetyl cellulose resins. Resin, cycloolefin polymer resin, polyethersulfone resin, polycarbonate Resins based on polyolefins, polyamide resins, polyimide resins, polyamideimide resins, polyolefins resins, (meth)acrylic resins, polyvinyl chloride resins, polyvinylidene chloride resins fats, polystyrene resins, polyvinyl alcohol resins, polyarylate resins, Examples of the resin include light-transmitting resins such as phenylene sulfide resins and mixtures of these resins. Among them, acetyl cellulose resin, cycloolefin polymer resin, polyimide resin, etc. Among these, acetylene, acetylene-based, and polyamide-based resins are preferred, and among these, acetylene is more preferred from the viewpoint of high transparency. Cellulose-based resins, particularly triacetyl cellulose-based resins, are preferred, and they have flexibility. From this viewpoint, polyimide resins and polyamide resins are more preferable. If necessary, various additives such as a plasticizer, an ultraviolet absorbing agent, and a lubricant may be added.

[0055] Examples of polyester resins include polyethylene terephthalate (PET), poly Propylene terephthalate (PEN), polybutylene terephthalate, polyethylene naphtha Resins containing at least one type of tallow as a constituent component include polyester-based resins. It is known that when used in this way, it is excited and emits fluorescence when irradiated with ultraviolet light. This type of fluorescence can affect the color of the display surface, but optical films At 0, as mentioned above, light with a wavelength of 380 nm or less is almost completely blocked, so the light transmittance is Even if the base material 11 is made of polyester resin, the generation of fluorescence can be suitably prevented. This can be done.

[0056] Examples of acetyl cellulose resins include triacetyl cellulose resins and diacetyl cellulose resins. Triacetyl cellulose resins are suitable for use in the visible light range of 380°C. This resin is capable of achieving an average light transmittance of 50% or more at wavelengths up to 780 nm. The average light transmittance of the acetyl cellulose resin is preferably 70% or more, and more preferably 85% or more. I wish.

[0057] In addition to pure triacetyl cellulose, triacetyl cellulose resins include Cellulose such as cellulose acetate propionate and cellulose acetate butyrate As the fatty acid that forms an ester with the acetic acid, a component other than acetic acid may be used in combination. In addition, these triacetyl celluloses may be mixed with other compounds such as diacetyl cellulose, if necessary. A cellulose lower fatty acid ester may also be added.

[0058] Cycloolefin polymer resins include, for example, norbornene monomers and monocyclic Examples of the cycloolefin polymer-based substrate include polymers of cycloolefin monomers. Commercially available products include, for example, Zeonex and Zeonoa (Norborne) manufactured by Zeon Corporation. resin), SUMILITE FS-1700 manufactured by Sumitomo Bakelite Co., Ltd., JSR Corporation Arton (modified norbornene resin) manufactured by Mitsui Chemicals, and APEL (cyclic olefin resin) manufactured by Mitsui Chemicals. (cyclic olefin copolymer), Ticona's Topas (cyclic olefin copolymer), Hitachi Chemical Co., Ltd. Examples include the Optretz OZ-1000 series (alicyclic acrylic resin) manufactured by Epson Corporation. .

[0059] Examples of polycarbonate resins include bisphenols (such as bisphenol A). Aromatic polycarbonate based on diethylene glycol bisallyl carbonate and the like aliphatic polycarbonates.

[0060] Examples of the (meth)acrylic resin include poly(methyl(meth)acrylate), poly(meth)acrylate, p) Ethyl acrylate, methyl (meth)acrylate-butyl (meth)acrylate copolymer etc.

[0061] Examples of polyimide resins include compounds having a structure represented by the following formula: In the following formula, n is a repeating unit and represents an integer of 2 or more.

[0062] [ka]

[0063] [ka]

[0064] [ka]

[0065] [ka]

[0066] [ka]

[0067]

change

[0068]

change

[0069]

change

[0070]

change

[0071]

change

[0072]

change

[0073]

change

[0074]

change

[0075]

change

[0076]

change

[0077] [ka]

[0078] [ka]

[0079] Polyamide resins include not only aliphatic polyamides but also aromatic polyamides (aramids). Polyamide resins are generally represented by the following formulas (18) and (19): The polyamide resin has a skeleton represented by the following formula ( 20) In the following formula, n is a repeating unit, and Represents an integer greater than or equal to 1.

[0080] [ka]

[0081] [ka]

[0082] [ka]

[0083] Polyimide resins or polyamides represented by the above formulas (1) to (17) and (20) The substrate made of the polyimide-based resin may be a commercially available one. As a commercially available product of the above polyamide, for example, Neoprim manufactured by Mitsubishi Gas Chemical Co., Ltd. can be mentioned. Commercially available substrates made of ethylene-based resins include, for example, Miktron manufactured by Toray Industries, Inc. .

[0084] The thickness of the light-transmitting substrate 11 is not particularly limited, but is preferably 250 μm or less. If the thickness of the light-transmitting substrate 11 is 250 μm or less, the flexibility of the optical film can be ensured. The lower limit of the thickness of the light-transmitting substrate 11 is the optical filter. From the viewpoint of improving the mechanical strength of the film 10, the thickness of the light-transmitting substrate 11 is preferably 10 μm or more. The upper limit is more preferably 125 μm or less, and even more preferably 115 μm or less. The thickness of the light-transmitting substrate is preferably 100 μm or less, and most preferably 100 μm or less. A cross section of the light-transmitting substrate is photographed using a scanning electron microscope (SEM), and the light The thickness of the transparent substrate is measured at 20 points, and the arithmetic average value of the thicknesses at the 20 points is calculated. It should be noted that the photographing with a scanning electron microscope depends on the thickness of the light-transmitting substrate. This is done at an appropriate magnification, with the interface line between the light-transmitting substrate and the light-transmitting functional layer clearly defined. Specifically, for example, when the thickness of the light-transmitting substrate is 50 μm, the magnification is 1000 times, In addition, the magnification is adjusted appropriately depending on the thickness of the light-transmitting substrate, such as 500 times for a 100 μm substrate. do.

[0085] The light-transmitting substrate 11 is previously subjected to a surface treatment such as sputtering, corona discharge, ultraviolet irradiation, or electron beam irradiation. The plate may be subjected to etching treatments such as glazing, chemical conversion, oxidation, etc., or to undercoating treatments. By being applied in advance, the adhesiveness with the light-transmitting functional layer formed on the light-transmitting substrate is improved. In addition, before forming the light-transmitting functional layer, etc., a solvent may be added as necessary. The surface of the light-transmitting substrate may be cleaned and purified by washing, ultrasonic washing or the like.

[0086] <<<Light transparent functional layer>>> The light-transmitting functional layer 12 is a spectral transmittance adjusting layer 13 and a light-transmitting functional layer 14. The overcoat layer 14 is provided on the side opposite to the substrate 11. In the present embodiment, the light-transmitting functional layer 12 is composed of a spectral transmittance adjusting layer 13 and an overcoat layer 14. However, it may be composed of only the spectral transmittance adjusting layer 13 .

[0087] The thickness of the light-transmitting functional layer 12 is 9 μm or less. If the thickness exceeds 100 μm, the light-transmitting functional layer may crack due to strain stress. The film thickness of the light-transmitting functional layer is the thickness of the light-transmitting substrate and the light-transmitting functional layer as determined by the contrast difference in a microscope image. Since the interface line can be visually observed, the distance from this interface line to the surface of the light-transmitting functional layer can be measured. When the light-transmitting functional layer has a single-layer structure, the difference in contrast in a microscope image is Since the interface line between the light-transmitting substrate and the light-transmitting functional layer can be visually observed, the film thickness can be measured clearly. On the other hand, when the light-transmitting functional layer has a multi-layer structure, the interface line between the light-transmitting functional layers can be set. In this case, when the light-transmitting functional layer has a multi-layer structure, The "thickness of the light-transmitting functional layer" refers to the total thickness of each light-transmitting functional layer. The light-transmitting functional layer has a multi-layer structure, and the interface lines between the light-transmitting functional layers cannot be clearly identified. Even in this case, the thickness of the light-transmitting functional layer can be measured. The lower limit of the film thickness is 0.5 μm or more, from the viewpoint of maintaining the uniformity of the film thickness of the light-transmitting functional layer. It is preferable that the thickness is 1.5 μm or more, 2 μm or more, 2.5 μm or more, or 3 μm or more. The upper limit of the thickness of the light-transmitting functional layer 12 is 8 μm or less, 7 μm or less, or 6 μm or less. It is more preferable that the thickness of the light-transmitting functional layer is smaller (the smaller the value, the more preferable). A cross section of the light-transmitting functional layer was photographed using a scanning electron microscope (SEM). The thickness of the light-transmitting functional layer is measured at 20 points, and the arithmetic average value of the thicknesses at those 20 points is calculated. It can be calculated by:

[0088] The specific method for taking cross-sectional photographs is as follows. First, cut out a 1 mm x 10 mm piece. A block was prepared by embedding the optical film in an embedding resin, and a general By using a simple sectioning method, we cut uniform sections with a thickness of about 70 nm to 300 nm without holes. The sections were prepared using the Ultramicrotome EM UC7 (Leica Microsystems). The remaining uniform pieces without holes were then cut out. The block is used as the measurement sample. Then, the block is measured using a scanning electron microscope (SEM) (product name: S-4 A cross-sectional photograph of the measurement sample was taken using a microscope (Hitachi High-Technologies Corporation) When taking cross-sectional photographs using the S-4800, the detector is set to "SE" and the accelerating The cross-section was observed at a voltage of 3 kV and an emission current of 10 μA. Adjust the focus and observe the contrast and brightness to see if you can distinguish each layer. The exposure time is 100 to 100,000 times, preferably 1,000 to 10,000 times depending on the thickness of the light-transmitting functional layer. In order to reduce the measurement error of the film thickness, the film thickness of the light-transmitting functional layer is made as small as possible. For example, when the thickness of the light-transmitting functional layer is about 9 μm, For a diameter of about 5 μm, the magnification is preferably 2000 times, and for a diameter of about 5 μm, the magnification is preferably 2000 to 5000 times. , set the aperture to "Beam monitor aperture 1", set the objective lens aperture to "2", and also set the W. D. Set to "8mm".

[0089] <<Spectral transmittance adjustment layer>> The spectral transmittance adjusting layer 13 is a layer containing a resin and a spectral transmittance adjusting agent. The transmittance adjusting layer 13 contains, in addition to the resin and the spectral transmittance adjusting agent, inorganic particles, a leveling agent, and It may contain a polymerization initiator such as a radical polymerization initiator or a cationic polymerization initiator or its residue. .

[0090] The thickness of the spectral transmittance adjusting layer 13 is preferably 9 μm or less. If the thickness exceeds 9 μm, the spectral transmittance adjustment layer may crack due to strain stress. The thickness of the spectral transmittance adjusting layer 13 is determined in the same manner as the thickness of the light-transmitting functional layer 12. The lower limit of the thickness of the spectral transmittance adjusting layer 13 is 0.5 μm or more, 1 μm or more, More preferably, the optical fiber is 1.5 μm or more, 2 μm or more, 2.5 μm or more, or 3 μm or more. The upper limit of the thickness of the transmittance adjusting layer 13 is 8 μm or less, 7 μm or less, 6 μm or less, or 5 μm or less. It is more preferable that there is (the smaller the value, the better).

[0091] The hardness of the spectral transmittance adjusting layer 13 by the nanoindentation method (indentation hardness The thickness of the indene-based spectral transmittance adjusting layer 13 is preferably 120 MPa or more. If the stationary hardness is 120 MPa or more, the thickness variation in the surface can be suppressed and the optical This can prevent the occurrence of scratches on the optical film due to rubbing during handling. "Indentation hardness" refers to the hardness measured by the nanoindentation method. The hardness of the spectral transmittance adjusting layer 13 is measured when the tip is pressed with a maximum pressing load of 300 μN. The lower limit of the indentation hardness is preferably 200 MPa or more. The upper limit of the indentation hardness of the transmittance adjusting layer 13 is 400 MPa from the viewpoint of flexibility. It is preferable that the pressure is 300 MPa or less (the smaller the value, the better). If the layer is too soft, the indentation hardness cannot be measured, so the adhesive layer is It may not be possible to measure the axial hardness.

[0092] The indentation hardness was measured using the HYSITRON TI9 50 TriboIndenter. Specifically, first, The optical film was cut into a size of 10 mm x 10 mm and embedded in resin to create a block. A measurement sample suitable for hardness measurement using the nanoindentation method is prepared. The pulls were prepared using an ultramicrotome EM UC7 (Leica Microsystems). Next, as shown in FIG. 1, a light-transmitting functional layer is formed in a multi-layer structure. In some cases, for example, a cross section of such a measurement sample is observed using a scanning electron microscope (SEM). Observe whether the interface line between the spectral transmittance adjusting layer and the overcoat layer is clearly observed. In addition, when the light-transmitting functional layer has a single-layer structure, such a SEM observation is performed. Observation can be omitted. Next, the surface of the measurement sample that is pressed by the indenter is parallel to the stage mounting surface. The measurement sample was placed on a HYSITRON TI950 Tr. The specimen is then fixed on the stage of the iboIndenter. Then, the specimen is observed by SEM and the spectral transmittance is When the interface line between the refractive index adjusting layer and the overcoat layer is clearly observed, the spectral transmittance adjusting layer is The interface between the spectral transmittance adjusting layer and the overcoat layer is located at the flat area in the center of the layer. If the light is not clearly visible, the light-transmitting functional layer is pressed against the central flat portion of the functional layer in a load-controlled manner. The Berkovich indenter was moved at a speed of 10 nm / s so that the maximum indentation load was 300 μN. The specimen is then pushed into the measurement position at the maximum load, and then the maximum load is maintained for 5 seconds, after which the load is removed at the same speed. Then, the indentation depth h (nm) corresponding to the indentation load F (μN) at this time is continuously calculated. Measure and create a load-displacement curve. From the load-displacement curve, the maximum indentation load F max (N) is the projected area A where the indenter and the spectral transmittance adjustment layer are in contact p (mm 2 ) divided by The above A p is the contact point corrected for the indenter tip curvature by the standard method of the device. The indentation hardness is the arithmetic mean of the values ​​obtained by measuring at 10 points. The average value is taken.

[0093] <Resin> The resin contained in the spectral transmittance adjusting layer 13 includes a polymer of an ionizing radiation polymerizable compound. Resins include polymerized compounds polymerizable with ionizing radiation, solvent-drying resins, and heat-curing resins. The composition may contain a hydrophilic compound.

[0094] (Ionizing radiation polymerizable compound) The ionizing radiation polymerizable compound has at least one ionizing radiation polymerizable functional group. In this specification, the term "ionizing radiation polymerizable functional group" refers to a functional group that undergoes a polymerization reaction upon exposure to ionizing radiation. The ionizing radiation polymerizable functional group is, for example, (meth)acryloyl Examples of ethylenically unsaturated groups include aryl groups, vinyl groups, and allyl groups. The "(meth)acryloyl group" means an "acryloyl group" or a "methacryloyl group". The term "irradiated with ionizing radiation" refers to the ionizing radiation that is irradiated when polymerizing an ionizing radiation polymerizable compound. Radiation includes visible light, ultraviolet light, X-rays, electron beams, alpha rays, beta rays, and gamma rays. .

[0095] Examples of the ionizing radiation polymerizable compound having one ethylenically unsaturated group include ethyl ( (Meth)acrylate, Ethylhexyl (Meth)acrylate, Styrene, Methylstyrene Examples of the ethylene glycol esters having two or more ethylenically unsaturated groups include ethylene glycol esters having two or more ethylenically unsaturated groups, and N-vinylpyrrolidone. Examples of the radiation-polymerizable compound include polymethylolpropane tri(meth)acrylate. acrylate, hexanediol (meth)acrylate, tripropylene glycol di(meth)acrylate Acrylate, Diethylene glycol di(meth)acrylate, Pentaerythritol triacrylate (Meth)acrylate, Dipentaerythritol Hexa(meth)acrylate, 1,6- Hexanediol di(meth)acrylate, neopentyl glycol di(meth)acrylate or reaction products of the above-mentioned polyfunctional compounds with (meth)acrylates, etc. (For example, poly(meth)acrylate esters of polyhydric alcohols) .

[0096] In addition to the above compounds, a relatively low molecular weight polyester resin having an ethylenically unsaturated group is , polyether resin, acrylic resin, epoxy resin, urethane resin, alkyd resin, Pyroacetal resin, polybutadiene resin, polythiol polyene resin, etc. are also resistant to the above ionizing radiation. It can be used as a linear polymerizable compound.

[0097] The ionizing radiation polymerizable compound includes an ionizing radiation polymerizable monomer, an ionizing radiation polymerizable oligomer, and an ionizing radiation polymerizable terpolymer. A suitable polymer and / or ionizing radiation polymerizable prepolymer can be prepared and used. As the ionizing radiation polymerizable compound, from the viewpoint of obtaining excellent folding properties in the optical film, From this viewpoint, it is preferable to use at least an ionizing radiation polymerizable prepolymer. The polymerizable prepolymer may, for example, be an acrylic resin.

[0098] (Solvent drying type resin) Solvent-drying resins are resins that do not require solvents added to adjust the solid content during coating, such as thermoplastic resins. This resin becomes a coating simply by drying. By using it in combination with a solvent-drying resin, This effectively prevents film defects on the coated surface. The solvent drying type resin that can be used is not particularly limited, and generally, a thermoplastic resin is Resins can be used.

[0099] The thermoplastic resin is not particularly limited, and examples thereof include styrene-based resins, (meth)acrylic resins, and the like. vinyl acetate resin, vinyl ether resin, halogen-containing resin, alicyclic olefin resin, polycarbonate resin, polyester resin, polyamide resin, cellulosic resin Examples of the resin include a cellulose derivative, a silicone resin, and a rubber or elastomer.

[0100] The thermoplastic resin is amorphous and can be easily dissolved in an organic solvent (particularly, a mixture of multiple polymers and polymerizable compounds). In particular, it is preferable that the composition is soluble in a common solvent capable of dissolving the above-mentioned compounds. From the viewpoint of the above, styrene resins, (meth)acrylic resins, alicyclic olefin resins, polyethylene resins, etc. Preferred are steric resins, cellulose derivatives (such as cellulose esters), and the like.

[0101] (thermosetting compound) The thermosetting compound is not particularly limited, and examples thereof include phenol resin, urea resin, and diamine resin. phthalate resin, melamine resin, guanamine resin, unsaturated polyester resin, polyurethane ethane resin, epoxy resin, amino alkyd resin, melamine-urea co-condensation resin, silicon resin, polysiloxane resin, etc.

[0102] <Spectral transmittance adjuster> The spectral transmittance adjusting agent adjusts the spectral transmittance of the optical film 10. The refractive index adjusting layer 13 is formed of, for example, a sesamol-type benzotriazolyl group represented by the following general formula (21): 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl] ]-2H-benzotriazole (product name "Tinuvin 234", manufactured by BASF), 2 -(5-chloro-2-benzotriazolyl)-6-tert-butyl-p-cresol ( Product name "Tinuvin 326" manufactured by BASF) or other ultraviolet absorbents, dyes and facial When a pigment material such as a pigment is contained, the above-mentioned spectral transmittance can be suitably satisfied. Among these, the above-mentioned spectrum slope is large and it blocks blue light more selectively. This makes it possible to block blue light while suppressing the increase in the YI value. From this viewpoint, a sesamol-type benzotriazole monomer represented by the following general formula (21) is preferred. As for UV absorbents, in addition to benzotriazole type, benzophenone type and triazole type are also available. As the dye material, for example, the UV absorber manufactured by Orient Chemical Industries, Ltd. Indole-based materials such as BONASORB UA-3911 and UA-3912 manufactured by Orient Chemical Industry Co., Ltd. Azomethine-based materials such as BONASORB UA-3701 manufactured by BASF, Lumogen manufactured by BASF, etc. Also use F Violet 570, Tinuvin Carboprotect, etc. can be done. [ka] In the formula, R 1 R represents a hydrogen atom or a methyl group. 2 is a straight or branched chain having 1 to 6 carbon atoms or a linear or branched oxyalkylene group having 1 to 6 carbon atoms.

[0103] The sesamol-type benzotriazole monomer is not particularly limited, but specific examples include The substance name is 2-[2-(6-hydroxybenzo[1,3]dioxol-5-yl )-2H-benzotriazol-5-yl]ethyl methacrylate, 2-[2-(6-Hydroxyethyl hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazole-5- 3-[2-(6-hydroxybenzo[1,3]dioxole -5-yl)-2H-benzotriazol-5-yl]propyl methacrylate, 3-[ 2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazole 5-phenyl-5-yl]propyl acrylate, 4-[2-(6-hydroxybenzo[1,3 ]dioxol-5-yl)-2H-benzotriazol-5-yl]butyl methacrylate 4-[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H- Benzotriazol-5-yl]butyl acrylate, 2-[2-(6-hydroxybenzo Zo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yloxy] Ethyl methacrylate, 2-[2-(6-hydroxybenzo[1,3]dioxole-5 -yl)-2H-benzotriazol-5-yloxy]ethyl acrylate, 2-[3 -{2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzothiazolinone 2-[3-{2-( 6-Hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazole -5-yl}propanoyloxy]ethyl acrylate, 4-[3-{2-(6-hydroxy (benzo[1,3]dioxol-5-yl)-2H-benzotriazol-5-yl propanoyloxy]butyl methacrylate, 4-[3-{2-(6-hydroxybenzo [1,3]dioxol-5-yl)-2H-benzotriazol-5-yl}propano 2-[3-{2-(6-hydroxybenzo[1,3]yloxy]butyl acrylate Dioxol-5-yl)-2H-benzotriazol-5-yl}propanoyloxy ]ethyl methacrylate, 2-[3-{2-(6-hydroxybenzo[1,3]dioxo (2H-benzotriazol-5-yl)-2H-benzotriazol-5-yl}propanoyloxy]ethyl Acrylate, 2-(methacryloyloxy)ethyl 2-(6-hydroxybenzo[1, 3]dioxol-5-yl)-2H-benzotriazole-5-carboxylate, 2- (Acryloyloxy)ethyl 2-(6-hydroxybenzo[1,3]dioxole-5 -yl)-2H-benzotriazole-5-carboxylate, 4-(methacryloyl) 2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-butyl Benzotriazole-5-carboxylate, 4-(acryloyloxy)butyl 2-( 6-Hydroxybenzo[1,3]dioxol-5-yl)-2H-benzotriazole In addition, these sesamol-type benzotriesters can be used as esters of benzotriesters. The azole monomer may be used alone or in combination of two or more kinds.

[0104] Whether or not a spectral transmittance adjusting agent is present in the light-transmitting functional layer can be determined by, for example, infrared spectroscopy or Raman spectroscopy. Spectroscopy, pyrolysis gas chromatography mass spectrometry, liquid chromatography mass spectrometry This can be confirmed by analytical methods such as X-ray photoelectron spectroscopy and TOF-SIMS.

[0105] The spectral transmittance adjusting agent may be, as long as it satisfies the requirements for the spectral transmittance described above. The refractive index adjusting layer 13 may be contained in any state. The above-mentioned spectral transmittance adjusting agent is contained in the transparent functional layer to satisfy the above-mentioned requirements for the spectral transmittance. Alternatively, the function of satisfying the above-mentioned requirements for spectral transmittance may be shared among a plurality of layers.

[0106] As an example of a structure in which the function of satisfying the above-mentioned requirements for spectral transmittance is shared among multiple layers, In the case where the light transmittance adjusting layer is composed of two layers, a first spectral transmittance adjusting layer and a second spectral transmittance adjusting layer, In this case, the first spectral transmittance adjusting layer can achieve only the spectral transmittance at a wavelength of 380 nm. The second spectral transmittance adjusting layer contains the above-mentioned spectral transmittance adjusting agent and has a wavelength of 410 nm. The above spectral transmittance conditions at wavelengths of 440 nm and 450 nm can be achieved. The spectral transmittance adjusting layer may be formed of three or more layers. The spectral transmittance adjusting layers are each configured to adjust the spectral transmittance so as to satisfy the requirements for the spectral transmittance described above. It may also contain a stabilizer.

[0107] The spectral transmittance adjusting agent may be present in the spectral transmittance adjusting layer 13 in an amount of, for example, 0.05% by mass or more to 50% by mass. The spectral transmittance adjuster may be contained in an amount of 0.1% by mass or less. By doing so, the above-mentioned spectral transmittance can be satisfied.

[0108] The spectral transmittance adjusting agent is used in the spectral transmittance adjusting layer 13. The resin may react with the resin constituting the spectral transmittance adjusting layer 13 and be contained therein integrally. It may be contained alone without reacting with the resin.

[0109] The spectral transmittance adjusting agent is reacted with the resin constituting the spectral transmittance adjusting layer 13 to be integrated therewith. Specifically, the spectral transmittance adjusting layer 13 may be, for example, a material having the above-mentioned spectral transmittance adjusting agent, Samol-type benzotriazole monomer is designated as A, and methyl methacrylate (MMA) is designated as B. , and other UV absorbents (for example, Otsuka Chemical's "RUVA93" and Shipro Chemical's "SEE When A is C, A, B, and C are acrylic or acrylic When the compounding ratio of A is X parts by mass, X is 10 to 55 A composition for a light-transmitting functional layer comprising 90 parts by mass of a polymer (a polymer that is 10 parts by mass of a PETA) and 10 parts by mass of a PETA. The spectral transmittance adjusting layer 1 thus obtained may be formed using a material such as a fluorine-containing compound. The optical film 10 having the above-mentioned spectral transmittance can be obtained. The shielding performance is excellent.

[0110] The spectral transmittance adjusting layer 13 is formed by, for example, using an ionizing radiation polymerizable compound and a spectral transmittance adjusting agent. A composition for a spectral transmittance adjusting layer containing the above-mentioned compound is applied to one surface 11A of the light-transmitting substrate 11 and dried. The resin can be formed by curing the resin by irradiating it with ionizing radiation. .

[0111] <Composition for spectral transmittance adjustment layer> The composition for the spectral transmittance adjusting layer contains, in addition to the ionizing radiation polymerizable compound and the spectral transmittance adjusting agent, It may contain a solvent drying type resin, a thermosetting compound, a polymerization initiator, a solvent, and the like.

[0112] (Polymerization initiator) The polymerization initiator is not particularly limited, and any known polymerization initiator can be used. For example, Specific examples of initiators include acetophenones, benzophenones, and Michler's benzoyl. Benzoates, α-amyloxime esters, thioxanthones, propiophenones, Examples of photosensitizers include benzils, benzoins, and acylphosphine oxides. It is preferable to use a mixture of these. Specific examples of such a mixture include n-butylamine and trimethylamine. Examples thereof include ethylamine and poly-n-butylphosphine.

[0113] As the polymerization initiator, when the ionizing radiation polymerizable compound has a radical polymerizable functional group, In this case, acetophenones, benzophenones, thioxanthones, benzoin, benzoyl It is preferable to use a radical polymerization initiator such as dimethyl ether alone or in combination. Among dialkyl polymerization initiators, 2,4, 6-Trimethylbenzoyldiphenylphosphine oxide (e.g., IGM Resin Omnirad TPO manufactured by ns BV), Bis(2,4,6-trimethylbenzoyl phenylphosphine oxide (e.g., Om nirad819), 1-hydroxycyclohexyl phenyl ketone (e.g., IGM Resins BV's Omnirad 184), or a mixture of these, preferable.

[0114] In addition, when the ionizing radiation polymerizable compound has a cationic polymerizable functional group, the polymerization initiator The agents include aromatic diazonium salts, aromatic sulfonium salts, aromatic iodonium salts, Cationic polymerization initiators such as thalocene compounds and benzoin sulfonate esters can be used alone or in combination. Among the cationic polymerization initiators, the following is preferably used in view of its excellent curability: Aromatic sulfonium salts and the like are more preferred.

[0115] The content of the polymerization initiator in the composition for the spectral transmittance adjusting layer is It is preferable that the amount is 1 part by mass or more and 10 parts by mass or less relative to 100 parts by mass of fat. If the content is less than 10 parts by mass, the hardness of the spectral transmittance adjusting layer may be insufficient. If this happens, ionizing radiation will not reach the depths of the applied film, and internal curing will not be promoted, resulting in the failure to achieve the desired results. There is a risk that the hardness of the surface of the optical film (for example, pencil hardness of B or higher, as described later) may not be achieved. be.

[0116] The lower limit of the content of the photopolymerization initiator is more preferably 2 parts by mass or more, and the upper limit is preferably 8 parts by mass or more. It is more preferable that the content of the photopolymerization initiator is within this range. As a result, no distribution of hardness occurs in the film thickness direction, and the hardness tends to be uniform.

[0117] (solvent) The solvent is selected according to the type and solubility of the ionizing radiation polymerizable compound used. For example, ketones (acetone, methyl ethyl ketone, methyl isobutene, chiroketone, cyclohexanone, diacetone alcohol, etc.), ethers (dioxane, Tetrahydrofuran, propylene glycol monomethyl ether, propylene glycol Monomethyl ether acetate, etc.), aliphatic hydrocarbons (hexane, etc.), alicyclic hydrocarbons (cyclohexane, etc.), aromatic hydrocarbons (toluene, xylene, etc.), halogenated carbons (dichloromethane, dichloroethane, etc.), esters (methyl acetate, ethyl acetate, acetic acid butyl, etc.), water, alcohols (ethanol, isopropanol, butanol, cyclohexane xanol, etc.), cellosolves (methyl cellosolve, ethyl cellosolve, etc.), cellosolve Acetates, sulfoxides (dimethyl sulfoxide, etc.), amides (dimethylformamide, amide, dimethylacetamide, etc.) and the like, and a mixed solvent of these may also be used.

[0118] The content ratio (solid content) of the raw materials in the composition for the spectral transmittance adjusting layer is not particularly limited. However, the content is preferably 5% by mass or more and 70% by mass or less, and more preferably 15% by mass or more and 60% by mass or less. I wish.

[0119] The composition for the spectral transmittance adjusting layer has properties to increase hardness, suppress cure shrinkage, and control the refractive index. and / or antiglare properties, etc., according to the purpose, a conventionally known dispersant, surfactant, etc. , antistatic agents, silane coupling agents, thickeners, coloring inhibitors, colorants (pigments, dyes), extinguishing agents Foaming agents, leveling agents, flame retardants, UV absorbers, adhesion promoters, polymerization inhibitors, antioxidants, surface A surface modifier, a lubricant, etc. may be added.

[0120] The composition for the spectral transmittance adjusting layer may be used by mixing a photosensitizer. Specific examples of the photosensitizer include Examples of the amine include n-butylamine, triethylamine, and poly-n-butylphosphine. can be done.

[0121] The method for preparing the composition for the spectral transmittance adjusting layer is not particularly limited as long as each component can be mixed uniformly. For example, known devices such as a paint shaker, a bead mill, a kneader, a mixer, etc. It can be done using.

[0122] The method for applying the composition for the spectral transmittance adjusting layer onto the light-transmitting substrate 11 is not particularly limited. For example, a spin coating method, a dip coating method, a spray method, a die coating method, a bar coating method, Roll coater method, meniscus coater method, flexographic printing method, screen printing method, pied Examples of the method include a known method such as a coater method.

[0123] The ionizing radiation source used for curing the composition for the spectral transmittance adjusting layer is mainly 190 to 4 The ionizing radiation source preferably has an emission peak in the wavelength region of 50 nm. , Ultra-high pressure mercury lamp, High pressure mercury lamp, Low pressure mercury lamp, Carbon arc lamp, Black light fluorescent lamp, Examples of light sources include metal halide lamps.

[0124] <<Overcoat layer>> The overcoat layer 14 provides a hard coat property to the surface 10A of the optical film 10. The layer has the function of providing a hard coat with a hardness of "B" or higher in the pencil hardness test. The pencil hardness test is carried out on a specimen cut to a size of 50 mm x 100 mm. The surface of the overcoat layer of the optical film was subjected to a pencil hardness tester (product name: Pencil Scratch Coating A film hardness tester (electric type, manufactured by Toyo Seiki Seisakusho Co., Ltd.) was used to measure the hardness of the film using a pencil (product name: Uni ", manufactured by Mitsubishi Pencil Co., Ltd.) was subjected to a load of 2.94 N while moving the pencil at a speed of 1 mm / sec. The pencil hardness is measured by moving the optical filter with a pencil. The hardness is the highest hardness that does not scratch the surface of the overcoat layer of the film. When measuring, multiple pencils with different hardness are used, and each pencil is tested five times. If the surface of the overcoat layer is not scratched in at least four out of five tests, It is judged that the surface of the overcoat layer is not scratched by the pencil having a hardness of 100 mm or less. is visually observed by observing the surface of the overcoat layer subjected to the pencil hardness test under a fluorescent lamp. Refers to something.

[0125] The thickness of the overcoat layer 14 is preferably 1 μm or more and less than 9 μm. If the thickness of the coating layer is less than 1 μm, the desired hardness may not be obtained. If the thickness of the overcoat layer is 9 μm or more, the overcoat layer will crack due to strain stress. The thickness of the overcoat layer 14 is determined in the same manner as the spectral transmittance adjusting layer 13. It can be calculated by:

[0126] The overcoat layer 14 may be made of a resin. The resin contained in the above-mentioned is a polymer of an ionizing radiation polymerizable compound. In addition to the polymerized products of ionizing radiation polymerizable compounds, solvent-drying resins and thermosetting compounds may also be included. good.

[0127] The ionizing radiation polymerizable compound constituting the overcoat layer 14 may be an ionizing radiation polymerizable compound. The polymerizable monomer may be an ionizing radiation polymerizable oligomer or an ionizing radiation polymerizable prepolymer. The ionizing radiation polymerizable compound may be, for example, an ionizing radiation polymerizable compound such as an ionizing radiation polymerizable compound. A radiation-polymerizable monomer and an ionizing radiation-polymerizable oligomer or an ionizing radiation-polymerizable prepolymer are A combination with a ribbon is preferred.

[0128] Examples of the ionizing radiation polymerizable monomer include 2-hydroxyethyl (meth)acrylate. acrylate, 2-hydroxypropyl (meth)acrylate, 2-ethylhexyl (meth)acrylate Monomers containing hydroxyl groups such as acrylate, ethylene glycol di(meth)acrylate, di Ethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate acrylate, tetraethylene glycol di(meth)acrylate, tetramethylene glycol Di(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolpropane Rolethane tri(meth)acrylate, Pentaerythritol di(meth)acrylate , Pentaerythritol tri(meth)acrylate, Pentaerythritol tetra(meth)acrylate ) acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol (Meth)acrylates such as glycerol hexa(meth)acrylate and glycerol (meth)acrylate Examples of the acrylic acid esters include acrylic acid esters.

[0129] The ionizing radiation polymerizable oligomer is preferably a polyfunctional oligomer having two or more functional groups. A polyfunctional oligomer having three or more (trifunctional) radiation-polymerizable functional groups is preferred. Examples of oligomers include polyester (meth)acrylate and urethane (meth)acrylate. Acrylate, polyester-urethane (meth)acrylate, polyether (meth)acrylate acrylate, polyol (meth)acrylate, melamine (meth)acrylate, isocyanate Examples thereof include nurate (meth)acrylate and epoxy (meth)acrylate.

[0130] The ionizing radiation polymerizable prepolymer has a weight-average molecular weight of more than 10,000. The average molecular weight is preferably from 10,000 to 80,000, and more preferably from 10,000 to 40,000. If the average molecular weight exceeds 80,000, the viscosity will be high and the coating suitability will decrease, resulting in The appearance of the light-transmitting resin may be deteriorated. (Meth)acrylate, Isocyanurate (Meth)acrylate, Polyester-urethane (meth)acrylate, epoxy (meth)acrylate, etc.

[0131] The overcoat layer 14 is, for example, a coating composition for an overcoat layer containing an ionizing radiation polymerizable compound. The composition is applied onto the spectral transmittance adjusting layer, dried, and cured by irradiating with ionizing radiation. It can be formed by converting the

[0132] <Composition for overcoat layer> The composition for the overcoat layer includes ionizing radiation polymerizable compounds, solvent drying resins, and heat curable resins. The resin may contain a solvent-drying type resin, a thermosetting compound, a polymerization initiator, a solvent, etc. The polymerization initiator, the solvent, and the like are the same as those described above for the composition for the spectral transmittance adjusting layer, as well as the solvent drying type resin and the heat curing type resin. The chemical compounds, polymerization initiators, solvents, etc. are the same, and therefore the description thereof will be omitted here. .

[0133] The light-transmitting functional layer 12 shown in FIG. 1 is made up of a spectral transmittance adjusting layer 13 and an overcoat layer 14. It has a two-layer structure, but the light-transmitting functional layer is a spectral transmittance adjusting layer and an overcoat layer. and an antifouling layer provided on the side of the overcoat layer opposite to the light-transmitting substrate side. The light-transmitting functional layer may be an overcoat. In the case where the light transmitting functional layer does not include the spectral transmittance adjusting layer, the light transmitting functional layer is Other light-transmitting functional layers such as an antifouling layer provided on the surface opposite to the light-transmitting substrate side In these cases, the spectral transmittance adjusting layer and the overcoat layer may be The antifouling layer is the same as the transmittance adjusting layer 13 and the overcoat layer 14. The surface of the image display device used was stained with dirt (fingerprints, water-based or oil-based inks, pencils, etc.). This layer plays a role in preventing dirt from adhering to the surface, and in the event that dirt does adhere to the surface, making it easy to wipe off the dirt. In addition, the formation of the antifouling layer improves the antifouling and scratch resistance of the optical film. It is also possible.

[0134] The antifouling layer includes, for example, an antifouling agent and a resin. Its main purpose is to prevent the surface from getting dirty, but it can also provide scratch resistance to optical films. do.

[0135] The antifouling agent may be, for example, a fluorine-based compound, a silicon-based compound, or a mixture thereof. More specifically, 2-perfluorooctylethyltriaminosilane Silane coupling agents having a fluoroalkyl group such as silane coupling agents having an amino group are particularly preferred. The resin is not particularly limited, and the above-mentioned Examples of the resin include those described in the section on the spectral transmittance adjusting layer 13.

[0136] The antifouling layer is preferably formed so that the antifouling layer is the outermost surface. For example, it can be substituted by imparting antifouling properties to the spectral transmittance adjusting layer itself.

[0137] <<<Other optical films>>> As shown in FIG. 3, the optical film is made up of a light-transmitting substrate 11 and a light-transmitting layer 12. The optical film 20 may be provided with a light-transmitting functional layer 21 provided on one surface side. Since the surface 21A of the light-transmitting functional layer 21 is an uneven surface, for example, the optical film 2 The optical film 20 can be provided with antiglare properties and / or anti-blocking properties. The light-transmitting substrate 11 in the optical film 10 is the same as the light-transmitting substrate 11 described in the section on the optical film 10. Therefore, the description will be omitted.

[0138] The physical properties of the optical film 20 are similar to those of the optical film 10. The spectral transmittance at wavelength 380 nm is also less than 1% in the 20-nm model. The spectral transmittance at 10 nm is 10% or more but less than 60%, and the wavelength is 440 nm. The spectral transmittance is 70% or more.

[0139] <<Light transparent functional layer>> The light-transmitting functional layer 21 has a function of adjusting the spectral transmittance of the optical film 20. The light-transmitting functional layer 21 has a spectral transmittance adjusting function. The light transmitting function can be exhibited by adding the above-mentioned spectral transmittance adjusting agent. The antiglare function of the layer 21 can be exhibited by making the surface 21A an uneven surface. For example, by incorporating an anti-glare agent, the surface 21 can be made uneven. There are no particular limitations on the type of particles, and various known inorganic or organic particles can be used.

[0140] The above particles may be either spherical particles or irregularly shaped particles. The term "spherical particles" used herein means, for example, particles in the shape of a perfect sphere, an oval sphere, etc., and the term "irregular shaped particles" means, It means a particle having a potato-like shape with random unevenness on the surface. The above particles are spherical particles. In the case of a child, a spherical one is preferable.

[0141] The average particle size of the above particles is not particularly limited, but is generally 0.01 μm or more. The average particle size of the above particles is measured by scanning electron microscope (SEM), transmission Particles photographed using a transmission electron microscope (TEM) or a scanning transmission electron microscope (STEM) The particle sizes of 20 particles were measured from the cross-sectional image, and the arithmetic mean value of the particle sizes of the 20 particles was calculated. However, if the particles are irregularly shaped, the particle diameter of each particle shall be the longest diameter in the cross section. The diameter shall be the average of the longest and shortest diameters.

[0142] The above particles exhibit antiglare properties and are preferably transparent particles. Specific examples of such fine particles include inorganic particles such as silica beads, and organic particles such as An example is plastic beads.

[0143] Specific examples of the plastic beads include styrene beads (refractive index 1.60 ), melamine beads (refractive index 1.57), acrylic beads (refractive index 1.49), acrylic -Styrene beads (refractive index 1.54), polycarbonate beads, polyethylene beads, etc. Examples include:

[0144] In the light-transmitting functional layer 21, the average interval between the projections and recesses on the surface 21A is defined as Sm, and the average The average inclination angle was θa, the arithmetic mean roughness of the unevenness was Ra, and the ten-point mean roughness of the unevenness was Rz. In this case, anti-glare performance is ensured by making only the edges of the reflected image less visible. In addition, by eliminating large diffusion and preventing stray light, it is possible to provide a suitable amount of regular transmission. The present invention provides an optical film that provides a bright image and has excellent contrast in both a bright room and a dark room. From this viewpoint, it is preferable that Sm satisfies the following formulae (A-1) to (A-4). If the amount is less than the lower limit of A-1), it may be difficult to control the aggregation, and Sm may not be expressed by the following formula: (A-1) If the upper limit is exceeded, the image may not be able to reproduce fine details and may appear rough. In addition, when θa, Ra, and Rz are within the lower limits of the following formulas (A-2) to (A-4), If it is less than θa, Ra, it may not be possible to suppress the reflection of external light. When Rz exceeds the upper limit of the following formulas (A-2) to (A-4), the regular transmission component decreases, causing the image to blur. The brightness is reduced, the bright room contrast is reduced due to the increase in diffuse reflection of external light, and the transmitted image light There is a risk that the darkroom contrast will decrease due to an increase in stray light from the 50μm <Sm<600μm …(A-1) 0.1°<θa<1.5° …(A-2) 0.02μm <Ra<0.30μm …(A-3) 0.30μm <Rz<2.00μm …(A-4)

[0145] From the above viewpoint, the surface 21A of the light-transmitting functional layer 21 is represented by the following formulae (B-1) to (B-4). It is more preferable to satisfy 100μm <Sm<400μm …(B-1) 0.1°<θa<1.2° …(B-2) 0.02μm <Ra<0.15μm …(B-3) 0.30μm <Rz<1.20μm …(B-4)

[0146] The surface 21A of the light-transmitting functional layer 21 preferably satisfies the following formulae (C-1) to (C-4): More preferred. 120μm <Sm<300μm …(C-1) 0.1°<θa<0.5° …(C-2) 0.02μm <Ra<0.12μm …(C-3) 0.30μm <Rz<0.80μm …(C-4)

[0147] In this specification, the above Sm, Ra and Rz are in accordance with JIS B0601:1994. The value of θa is obtained by a method based on the surface roughness measurement instrument SE-3400 (K.K.) The definition is given in the instruction manual (revised on July 20, 1995) of the Kosaka Laboratory Co., Ltd. As shown in Figure 4, the sum of the heights of the protrusions that exist over the reference length L (h 1 +h 2 +h 3 +···+h n ) arctangent θa=tan -1 {(h 1 +h 2 +h 3 +···+h n ) / L}. Such Sm, θa, Ra, and Rz are obtained, for example, by measuring surface roughness. Using a container (product name "SE-3400", manufactured by Kosaka Laboratory Co., Ltd.), a light-transmitting functional layer 21 On the surface 21A, at least a portion that is visually normal (no large foreign objects, scratches, etc.) Three points were randomly selected (points where the sample was not exposed) and the arithmetic mean value of the values ​​measured at those points was calculated. The measurement conditions in this case are Ra on the surface 10A of the optical film 10 and In addition, Ra is an interatomic ratio similar to Ra on the surface 10A of the optical film 10. Measurements can also be made using a force microscope (product name "WET-9100", manufactured by Shimadzu Corporation).

[0148] When the light-transmitting functional layer 21 has blocking resistance, the light-transmitting functional layer 21 is, for example, For example, it is preferable to contain an antiblocking agent. For example, aluminum oxide, magnesium oxide, silica, calcium oxide, titanium oxide, Oxides such as zinc, hydroxides such as aluminum hydroxide, magnesium hydroxide, and calcium hydroxide hydrates, magnesium carbonate, carbonates such as calcium carbonate, calcium sulfate, barium sulfate, etc. sulfates, magnesium silicate, aluminum silicate, calcium silicate, aluminosilicate One or more inorganic compounds such as silicates of acids, kaolin, talc, diatomaceous earth, etc. There are two or more types.

[0149] The average particle size of the inorganic compound-based antiblocking agent is 0.01 μm or more and 20 μm or less. When the average particle size of the antiblocking agent is less than 0.01 μm, the antiblocking agent is easily absorbed by the photosensitive resin. The surface irregularities of the permeable functional layer are small, making it difficult to obtain an anti-blocking effect. If the average particle size exceeds 20 μm, the surface irregularities of the light-transmitting functional layer become too large, resulting in poor optical properties. When films rub against each other, scratches and other marks may occur.

[0150] Examples of the blocking inhibitor include high density polyethylene, molecular weight of 300,000 or more. Ultra-high molecular weight polyethylene, polypropylene, polycarbonate, polyamide, polyester From fine powders of resins such as melamine resin, diallyl phthalate resin, acrylic resin, etc. The raw material may be one or more organic compounds such as the above.

[0151] The content of the anti-blocking agent is based on 100 parts by mass of the resin constituting the light-transmitting functional layer. , preferably 0.01 parts by mass or more and 6 parts by mass or less, and more preferably 2 parts by mass or more and 5 parts by mass or less. It is more preferable that the content of the antiblocking agent is less than 0.01 parts by mass. The unevenness of the surface of the light-transmitting functional layer is insufficient, and the blocking resistance is insufficient. If the content exceeds 6 parts by mass, the transparency of the light-transmitting functional layer may decrease. .

[0152] <<<Other optical films>>> As shown in FIG. 5, the optical film is made up of a light-transmitting substrate 11 and a light-transmitting layer 12. The optical film 30 may be provided with a light-transmitting functional layer 31 on one surface side. The light-transmitting functional layer 31 includes a spectral transmittance adjusting layer 32 and a light-transmitting layer in the spectral transmittance adjusting layer 32. The laminated structure includes a plurality of deposition layers 33 provided on the side opposite to the conductive substrate 11 side. By providing the deposition layer 33, the above-mentioned requirements for spectral transmittance can be more suitably met. do.

[0153] The physical properties of the optical film 30 are similar to those of the optical film 10. The spectral transmittance at wavelength 380 nm is also less than 1%. The spectral transmittance at 10 nm is 10% or more but less than 60%, and the wavelength is 440 nm. The spectral transmittance is 70% or more.

[0154] <<Spectral transmittance adjustment layer>> The spectral transmittance adjusting layer 32 is similar to the spectral transmittance adjusting layer 13, and therefore the description thereof will be omitted here. shall be abbreviated.

[0155] <<Vapour-deposited layer>> The deposition layer 33 may be made of, for example, silicon (Si), aluminum (Al), magnesium (Mg), or the like. (Mg), calcium (Ca), potassium (K), tin (Sn), sodium (Na), Boron (B), titanium (Ti), lead (Pb), zirconium (Zr), yttrium (Y It is preferable that the layer is a vapor-deposited layer of an inorganic substance such as niobium (Nb) or an inorganic oxide. Preferably, the deposited layer is made of silicon (Si) and niobium (Nb).

[0156] The deposition layer 33 is preferably a layer formed by a sputtering method. The deposition layer is formed by a sputtering method, so that the deposition layer can be formed by multi-layer thin film deposition. This allows for more precise control of film thickness.

[0157] The thickness of the deposition layer 33 is 3 nm or more and 150 nm or less, and 5 layers or more and 20 layers or less are laminated. By providing such a deposition layer 33 on the spectral transmittance adjusting layer 32, The film 30 prevents coloring caused by the vapor deposition layer 33 and more effectively meets the above-mentioned requirements for spectral transmittance. The thickness of each deposition layer can be measured by scanning electron microscope (SEM), transmission electron microscope (TEM), and The cross-section of the deposition layer was observed using a transmission electron microscope (TEM) or a scanning transmission electron microscope (STEM). The cross-sectional image was photographed, and the thickness of the deposition layer was measured at 20 points. The arithmetic mean value is used.

[0158] When photographing the cross section of a deposition layer using a TEM or STEM, the specific method for photographing the cross section is as follows: First, cut the optical film into pieces of 1 mm x 10 mm and embed it in an embedding resin. A block was prepared by embedding the specimen in the endothelial cell, and holes were cut from the block using a general sectioning method. Cut out uniform sections with a thickness of 70 nm to 100 nm. A microtome (EM UC7, Leica Microsystems, Inc.) was used. This uniform section without holes is used as the measurement sample. Transmission electron microscope (STEM) (product name: S-4800, Hitachi High-Technologies Corporation) The cross-section of the measurement sample is photographed using the S-4800. When taking the photograph, the detector was set to "TE", the acceleration voltage to "30 kV", and the emission current to " Set the current to 10μA and observe the cross section. Adjust the focus and contrast to obtain the magnification. Adjust the magnification and brightness appropriately at 5,000 to 200,000 times while observing whether each layer can be distinguished. The magnification is preferably 10,000 to 100,000 times, more preferably 10,000 to 50,000 times, and most preferably 10,000 to 50,000 times. The preferred magnification is 25,000 to 50,000 times. When taking a picture, set the aperture to "Beam monitor aperture 3" and the objective lens aperture You can also change the width to "3" and the working distance to "8 mm". By applying dyeing treatments such as ruthenium oxide and phosphotungstic acid, the interface lines between layers become easier to see. Therefore, dyeing treatment may be performed.

[0159] <<<Other optical films>>> As shown in FIG. 6, the optical film is made up of a light-transmitting substrate 11 and a light-transmitting layer 12. The optical film 40 may be provided with a light-transmitting functional layer 41 on one surface side. The light-transmitting functional layer 41 includes a spectral transmittance adjusting layer 42 and a light transmitting layer 43. A plurality of invisible layers 43 having different refractive indices are provided on the side opposite to the conductive substrate 11 side. The optical film 40 is preferably used in an image display device equipped with a touch panel. However, by having the invisible layer 43, it is possible to use an inorganic transparent conductive material such as ITO. The sensor electrode (transparent electrode layer) can be prevented from being observed on the display surface.

[0160] The physical properties of the optical film 40 are similar to those of the optical film 10. Even in the case of the 40-nm model, the spectral transmittance at a wavelength of 380 nm is less than 1%, and The spectral transmittance at 10 nm is 10% or more but less than 60%, and the wavelength is 440 nm. The spectral transmittance is 70% or more.

[0161] <<Spectral transmittance adjustment layer>> The spectral transmittance adjusting layer 42 is similar to the spectral transmittance adjusting layer 13, and therefore the description thereof will be omitted here. shall be abbreviated.

[0162] <<Invisible Layer>> The invisible layer 43 is not particularly limited, and examples thereof include those conventionally known invisible layers. However, for example, a high refractive index layer 43A having a refractive index higher than that of the inorganic transparent conductive material and a high refractive index layer It is preferable that the refractive index layer 43A has a laminated structure with a low refractive index layer 43B having a refractive index lower than that of the low refractive index layer 43A. The opaque layer 43 may be provided on both sides of the light-transmitting substrate 11 .

[0163] <High refractive index layer> The high refractive index layer 43A preferably has a refractive index of 1.50 or more and 2.00 or less. It is more preferable that the lower limit of the refractive index of the refractive index layer 43A is 1.60 or more, and the upper limit is 1. It is more preferable that the refractive index is 75 or less. The high refractive index layer 43A is scraped off with a cutter or the like to prepare a powder sample, which is then measured according to JIS K Becke method (refractive index is 0.01) according to 7142:2008, method B (for powder or granular transparent materials) Using the known Cargill reagent, the powder sample is placed on a slide glass or the like, and the The reagent is dropped onto the sample, and the sample is immersed in the reagent. The state is observed under a microscope. The difference in refractive index between the sample and the reagent causes a bright line (Beckhoff et al., 2013) at the sample outline. The refractive index of the reagent at which the line becomes invisible is taken as the refractive index of the sample. It shall be measured.

[0164] The thickness of the high refractive index layer 43A is preferably 10 nm or more and 200 nm or less. The lower limit of the thickness of the refractive index layer 43A is preferably 30 nm or more, and the upper limit is 100 nm or less. The thickness of the high refractive index layer 43A is preferably determined in the same manner as the thickness of the deposition layer 33. Therefore, we request this.

[0165] The high refractive index layer 43A is a layer having a refractive index higher than that of the inorganic transparent conductive material. There is no particular limitation as long as the layer is made of high refractive index fine particles and a binder resin. It is preferable to configure

[0166] Examples of the high refractive index fine particles include metal oxide fine particles. Examples of fine particles include titanium oxide (TiO 2 , refractive index: 2.3 to 2.7), nickel oxide Of (Nb 2 O 5 , refractive index: 2.33), zirconium oxide (ZrO 2 , Refractive Index: 2.1 0), antimony oxide (Sb 2 O 5, refractive index: 2.04), tin oxide (SnO 2 , refractive index : 2.00), tin-doped indium oxide (ITO, refractive index: 1.95 to 2.00), acid Cerium oxide (CeO 2 , refractive index: 1.95), aluminum doped zinc oxide (AZO, refractive index Refractive index: 1.90-2.00), Gallium-doped zinc oxide (GZO, Refractive index: 1.90-2 .00), Zinc Antimonate (ZnSb 2 O 6 , refractive index: 1.90~2.00), nitrogen oxide Lead (ZnO, refractive index: 1.90), yttrium oxide (Y 2 O 3 , Refractive index: 1.87), Antimony-doped tin oxide (ATO, refractive index: 1.75 to 1.85), phosphorus-doped tin oxide Among these, the refractive index of From this viewpoint, zirconium oxide is preferred.

[0167] The binder resin constituting the high refractive index layer 43A is not particularly limited. For example, From the viewpoint of increasing the degree of adhesion, a polymer (crosslinked material) such as a thermosetting resin or an ionizing radiation polymerizable compound is used. Among these, those which are polymers of ionizing radiation polymerizable compounds are preferred. As such a binder resin, the above-mentioned spectral transmittance adjusting layer 13 is preferably formed by using the above-mentioned binder resin. The resin components constituting the resin composition are the same as those constituting the resin composition.

[0168] The high refractive index layer 43A can be formed, for example, by the same method as that for the spectral transmittance adjusting layer 13. Specifically, for example, the surface of the spectral transmittance adjusting layer 42 on the light-transmitting base material 11 side is When the spectral transmittance adjusting layer 42 is formed on the opposite side, at least high refractive index fine particles are formed on the surface of the spectral transmittance adjusting layer 42. and a composition for a high refractive index layer, the composition comprising a thermosetting resin or an ionizing radiation polymerizable compound, is applied to form the layer. The resulting coating is dried, and then heated or irradiated with ionizing radiation such as ultraviolet light. The composition for high refractive index layer is then cured to form high refractive index layer 43A.

[0169] <Low refractive index layer> The low refractive index layer 43B is a layer having a refractive index lower than that of the high refractive index layer 43A. The refractive index of the low refractive index layer 43B is preferably 1.35 or more and 1.55 or less. The lower limit of the refractive index of the refractive index layer 43B is more preferably 1.40 or more, and the upper limit is preferably 1.50 or more. It is more preferable that the refractive index of the low refractive index layer 43B is lower than that of the high refractive index layer 43A. It shall be calculated in the same manner as above.

[0170] The low refractive index layer 43B preferably has a thickness of 1 nm or more and 200 nm or less. The lower limit of the thickness of the refractive index layer 43B is more preferably 5 nm or more, and the upper limit is 100 nm. The thickness of the low refractive index layer 43B is preferably set to a value equal to or smaller than the thickness of the deposition layer 33. The request shall be made by

[0171] The low refractive index layer 43B is, for example, made of low refractive index fine particles and a binder resin. and those made of low refractive index resins.

[0172] The low refractive index fine particles include, for example, silica or magnesium fluoride fine particles. Among them, hollow silica particles are preferred. The hollow silica particles can be produced, for example, by the method described in the examples of JP-A-2005-099778. It can be produced by the method.

[0173] The binder resin constituting the low refractive index layer 43B is the same as that constituting the high refractive index layer 43A. However, the binder resin may contain fluorine atoms. It is also possible to mix a material having a low refractive index, such as an introduced resin or organopolysiloxane. Examples of low refractive index resins include resins containing fluorine atoms and organopolysiloxane. Also included are resins with a low refractive index such as the above.

[0174] The low refractive index layer 43B may be formed, for example, by the same method as that for the spectral transmittance adjusting layer 13. Specifically, first, at least low refractive index fine particles are applied to the surface of the high refractive index layer 43A. and a composition for a low refractive index layer, the composition comprising a thermosetting resin or an ionizing radiation polymerizable compound. A film is formed, the coating film is dried, and then the coating film is heated or irradiated with ionizing radiation such as ultraviolet light. The composition for a low refractive index layer is cured in this manner to form the low refractive index layer 43B.

[0175] Between the high refractive index layer 43A and the low refractive index layer 43B, a layer having a refractive index lower than that of the high refractive index layer 43A is provided. The low refractive index layer 43B is provided with a medium refractive index layer having a refractive index higher than that of the low refractive index layer 43B. It's fine.

[0176] <<<Other optical films>>> As shown in FIG. 7, the optical film is made up of a light-transmitting substrate 11 and a light-transmitting layer 12. The optical film 50 may be provided with a light-transmitting functional layer 51 on one surface side. The light-transmitting functional layer 51 includes a spectral transmittance adjusting layer 52 and a light-transmitting layer in the spectral transmittance adjusting layer 52. The refractive index of the spectral transmittance adjusting layer 52 is lower than that of the spectral transmittance adjusting layer 53. It is preferable that the optical film 50 further includes a low refractive index layer 53. In addition, the optical film has a spectral transmittance adjusting layer. and a high refractive index layer having a refractive index higher than that of the spectral transmittance adjusting layer is provided between the low refractive index layer and the spectral transmittance adjusting layer. It may also be provided for.

[0177] The physical properties of the optical film 50 are similar to those of the optical film 10. Even in the case of the 40-nm model, the spectral transmittance at a wavelength of 380 nm is less than 1%, and The spectral transmittance at 10 nm is 10% or more but less than 60%, and the wavelength is 440 nm. The spectral transmittance is 70% or more.

[0178] <<Spectral transmittance adjusting layer and low refractive index layer>> The spectral transmittance adjusting layer 52 is similar to the spectral transmittance adjusting layer 13, and the low refractive index layer 53 is Since it is similar to the refractive index layer 43B, the description thereof will be omitted here.

[0179] The present inventors have conducted extensive research into the problem of yellowing of optical films and have found that If too much light is absorbed around 0 nm, the light passing through the optical film will have a yellowish tint. According to this embodiment, the optical films 10, 20, 30, and 40 have a wavelength of 380n The spectral transmittance at a wavelength of 410 nm is less than 1% and the spectral transmittance at a wavelength of 410 nm is 10% or more. The transmittance is less than 60% and the spectral transmittance at a wavelength of 440 nm is 70% or more. It absorbs light with a wavelength of 380 nm or less sufficiently and does not absorb too much light with a wavelength of around 410 nm. It is possible to transmit light with sufficient wavelengths of 440 nm or more. This makes it possible to block blue light and suppress the yellowish tint of the optical film.

[0180] In order to reliably fix the members together with the adhesive layer, the thickness of the adhesive layer is as described above. In contrast, the light-transmitting functional layers 12, 21, 31, Since the films 41 and 51 do not have an adhesive layer, the film thickness can be set to 9 μm or less. The thickness can be made thinner than when a spectral transmittance adjusting agent is included. The optical films 10, 20, 30, 40, and 50 can be made thinner. Since the rooms 10, 20, 30, 40, and 50 can be made thinner, the image display device can be made thinner. It is possible to achieve a smaller size and lighter weight.

[0181] When the adhesive layer contains a spectral transmittance adjuster, the adhesive strength decreases and the thermal shrinkage rate changes. As a result, there is a risk that the adherend may be deformed or the desired dimensions may not be obtained. Since the optical films 10, 20, 30, 40, and 50 do not have an adhesive layer, There is no problem. In addition, the optical films 10, 20, 30, 40, and 50 do not have an adhesive layer. So it's easy to use.

[0182] <<<Polarizing plate>>> The optical films 10, 20, 30, 40, and 50 can be incorporated into a polarizing plate. FIG. 8 is a schematic diagram of a polarizing plate according to this embodiment. As shown in FIG. The polarizing plate 60 includes an optical film 10, a polarizer 61, and a protective film 62 in this order. In addition, the polarizing plate 60 uses the optical film 10. Instead of the film 10, optical films 20, 30, 40, and 50 may be used. In FIG. 0, a polarizer 61 is provided on the light-transmitting substrate 11 side of the optical film 10. A polarizer may be provided on the light-transmitting functional layer side of the optical film.

[0183] The optical film 10 and the polarizer 61, and the polarizer 61 and the protective film 62 are, for example, water-based The polarizing plate 60 is attached to the polarizing plate 62 by means of an adhesive or an ultraviolet-curing adhesive. By using a circular polarizing plate as the polarizing plate 60, the organic light-emitting diode panel When used in an image display device equipped with an OLED panel, it can block external light. Cut.

[0184] <<Polarizer>> The polarizer 61 is disposed on the surface of the light-transmitting substrate 11 opposite to the surface on the light-transmitting functional layer 12 side. The polarizer 61 is a uniaxially stretched polarizer dyed with iodine or a dichroic dye. Examples of polyvinyl alcohol-based resins include polyvinyl alcohol-based resin films. The polyvinyl acetate resin may be saponified. Examples include polyvinyl acetate, which is a homopolymer of vinyl acetate, and vinyl acetate and its copolymer. Other monomers that can be copolymerized with vinyl acetate include copolymers with vinyl acetate and other monomers that can be copolymerized with vinyl acetate. Examples of the unsaturated carboxylic acids include unsaturated carboxylic acids, olefins, vinyl ethers, unsaturated sulfurs, and the like. Examples of the polyvinyl alcohol include polyvinyl alcohols having an ammonium group, and acrylamides having an ammonium group. The vinyl resin may be modified, for example, polyvinyl hol modified with aldehydes. Lumar, polyvinyl acetal, etc. can also be used.

[0185] <<Protective film>> The protective film 62 is, for example, a triacetyl cellulose film (TAC film). (meth)acrylic resin film, cycloolefin polymer film (COP), etc. Examples include:

[0186] <<<Image display devices>>> The optical films 10, 20, 30, 40, 50 or the polarizing plate 60 are incorporated into an image display device. FIG. 9 is a schematic diagram of an image display device according to this embodiment. As shown in FIG. 9, the image display device 70 includes a display panel 80 and a display panel 8 A touch sensor 90 is disposed on the observer side of the touch sensor 90. and a cover member 100 that constitutes a surface 70A of the image display device 70. .

[0187] The display panel 80 mainly comprises a display element 81, an adhesive layer 82, and a retardation filter 83 facing the viewer side. The film 83, the adhesive layer 84, the λ / 4 film 85, the adhesive layer 86, and the polarizing plate 60 are arranged in this order. The polarizing plate 60 is disposed so that the optical film 10 faces the viewer side. The display panel 80 has a display element 81 that is an organic light-emitting diode (OLED) element. The image display device 70 is configured as described above. However, the optical films 20, 30, 40, and 50 are used instead of the optical film 10. Good too.

[0188] As described above, the display element 81 is an organic light-emitting diode (OLED) element. The display element may be a liquid crystal display element, an inorganic light-emitting diode element, or a quantum dot light-emitting diode element. The adhesive layers 82 and 86 may be, for example, a pressure-sensitive adhesive. The adhesive layer 84 may be a liquid adhesive layer containing an ionizing radiation polymerizable compound. Examples include cured products of ionizing radiation curable adhesives (e.g., OCR: optically clear resin). can be.

[0189] A known touch sensor can be used as the touch sensor 90. 90 is disposed between the display panel 80 and the cover member 100, but the display element 81 and The cover member 100 may be disposed between the retardation film 83 and the cover glass. Alternatively, it may be a cover film made of a light-transmitting resin.

[0190] The display panel 80 and the touch sensor 90, and the touch sensor 90 and the cover member 100 are Adhesive layers 111 and 112 are made of a pressure-sensitive adhesive or a cured product of an ionizing radiation curable adhesive, respectively. However, between the display panel 80 and the touch sensor 90 and between the touch sensor Between the sensor 90 and the cover member 100, there may be an air layer (air gap). EXAMPLES

[0191] In order to explain the present invention in detail, the following examples are given. In addition, unless otherwise specified, "parts" or "%" in the text indicate the quantity. This is the quantity standard.

[0192] <Example 1> (Synthesis of Sesamol-type Benzotriazole Monomers) Equip a 200 mL four-neck flask with a ball condenser, mercury thermometer, and stirring device. , 6-[5-(2-hydroxyethyl)-2H-benzotriazol-2-yl]benzo [1,3]dioxol-5-ol 4.0 g (0.013 mol), toluene 40 mL, 1.8 g (0.021 mol) of methacrylic acid, 0.4 g (0.004 mol) of methanesulfonic acid ) was added and the mixture was refluxed at 110-115°C for 4 hours for dehydration. Add 0.6 g (0.006 mol) of sodium hydroxide, leave to stand, separate and remove the lower aqueous layer, and 0.2 g of charcoal was added, and the mixture was refluxed and stirred to remove color. After filtration, toluene was extracted from the filtrate. 40 mL was collected under reduced pressure, 100 mL of isopropyl alcohol was added, and the precipitated crystals were filtered. After filtration and washing with 40 mL of isopropyl alcohol, it was dried at 40°C under reduced pressure to obtain yellow crystals. The yellow crystals (4.2 g) were repulped and washed with isopropyl alcohol to obtain 4.2 g of the product. After drying at 40°C under reduced pressure, 3.4 g of 2 was obtained as a sesamol-type benzotriazole monomer. -[2-(6-hydroxybenzo[1,3]dioxol-5-yl)-2H-benzothiazolidinyl] riazol-5-yl]ethyl methacrylate was obtained.

[0193] (Synthesis of acrylic polymers with reactively bonded sesamol-type benzotriazole monomers) A Dimroth condenser, a mercury thermometer, a nitrogen gas inlet tube, and a stirrer were attached to the four-neck flask. The synthesized 2-[2-(6-hydroxybenzo[1,3]dioxol-5-yl 8 parts by mass of 2H-benzotriazol-5-yl]ethyl methacrylate, and other monomers 32 parts by mass of methyl methacrylate (MMA) as a substrate and 20 parts by mass of toluene as a solvent. 20 parts by mass of methyl ethyl ketone, and 1,1'-azobis( 0.6 parts by mass of cyclohexane-1-carbonitrile was added and the mixture was stirred with a nitrogen gas stream. After replacing the inside of the flask with nitrogen at a flow rate of 10 mL / min for 1 hour, the reaction mixture was heated to 90-96°C for 10 The polymerization reaction was carried out under reflux for 1 hour.

[0194] After the polymerization reaction was completed, 10 parts by mass of toluene and 10 parts by mass of MEK were added to obtain a sesamol-type benzoate. Acrylic polymer in which azotriazole monomer is reactively bonded to MMA and a UV absorber (1) 100.6 parts by mass of solution was obtained.

[0195] (Preparation of Spectral Transmittance Adjusting Layer Composition 1) Multifunctional monomer (product name "KAYARAD PET-30", manufactured by Nippon Kayaku Co., Ltd.) and and the above acrylic polymer (1) were mixed in a solid content mass ratio of 80:20, and the solid content was 25% The resin composition was diluted with a solvent (methyl ethyl ketone and toluene, mass ratio 80:20) until Next, a polymerization initiator (IGM Mass of Omnirad184 and Omnirad819 manufactured by Resins BV 4 parts by mass of 50:50 ratio) and 0 parts by mass of leveling agent (product name "F568", manufactured by DIC Corporation) 0.2 parts by mass and thoroughly stirred to prepare composition 1 for the spectral transmittance adjusting layer. Ta.

[0196] (Preparation of Overcoat Layer Composition 1) Multifunctional monomer (product name "KAYARAD PET-30", manufactured by Nippon Kayaku Co., Ltd.) , up to 50% solids, solvent (methyl ethyl ketone and methyl isobutyl ketone, mass ratio 5 The resin composition was then diluted with 200% water (0:50). Polymerization initiator (Omnirad184 manufactured by IGM Resins BV) 4 Mix 0.2 parts by weight of leveling agent (product name "F568", manufactured by DIC Corporation) with The mixture was mixed and thoroughly stirred to prepare a composition for the overcoat layer.

[0197] (Optical film manufacturing) The obtained composition 1 for the spectral transmittance adjusting layer was measured using a Maya bar to measure The surface of the triacetyl cellulose substrate was coated with a 25 μm thick film (A4 size). The coating film was then dried at 50° C. with a flow rate of 0.5 m / s. By passing air through the coating for 30 seconds, the solvent in the coating is evaporated, and the UV light is then turned on for 20 seconds. 0mJ / cm 2 The coating is then cured by irradiating it to a thickness of 5 μm. A transmittance adjusting layer was formed.

[0198] After forming the spectral transmittance adjusting layer, the surface of the spectral transmittance adjusting layer is overcoated with a meyer bar. The composition 1 for the undercoat layer was applied to form a coating film. Dry air at 70°C was passed through the coating at a flow rate of 1 / s for 30 seconds to evaporate the solvent in the coating. , the cumulative amount of ultraviolet light is 200 mJ / cm 2 The coating is then hardened by irradiating it until it becomes As a result, an overcoat layer having a thickness of 4 μm was formed. A 5μm thick spectral transmittance adjustment layer (SA layer) and a 4μm thick overcoat are applied to the substrate. An optical film having a light-transmitting functional layer having a thickness of 9 μm and consisting of an optically transparent layer (OC layer) was obtained. The thickness of the spectral transmittance adjustment layer was measured by observing the cross section of the spectral transmittance adjustment layer using a scanning electron microscope (SEM). The cross-sectional image was photographed, and the thickness of the spectral transmittance adjusting layer was measured at 20 points. The arithmetic average value of the thickness of the film was used. The specific method for taking the cross-sectional photographs was as follows. First, Optical film cut to 1 mm x 10 mm was embedded in embedding resin to create a block. Then, from this block, a uniform thickness of 70 nm to 100 nm was prepared by a general sectioning method without any holes. Sections of about 300 nm were cut. UC7" (Leica Microsystems, Inc.) was used. The remaining block from which uniform slices were cut was used as the measurement sample. A scanning electron microscope (SEM) (product name "S-4800", manufactured by Hitachi High-Technologies Corporation) was used. The cross-sectional photograph of the measurement sample was taken using the S-4800. In this case, set the detector to "SE", the acceleration voltage to "5 kV", and the emission current to "10 μA". The cross-section was observed by adjusting the focus and contrast and brightness. While observing whether each layer can be distinguished, the light-transmitting functional layer is magnified 1,000 to 10,000 times depending on the film thickness. Specifically, in order to reduce the measurement error of the film thickness, the light-transmitting functional layer In the case of 9 μm, the concentration was adjusted to 2000 times, and in the case of 5 μm, the concentration was adjusted to 2000 to 5000 times. , set the aperture to "Beam monitor aperture 1", set the objective lens aperture to "2", and also set the W. D was set to "8 mm". The thickness of the overcoat layer was also set to the same thickness as the spectral transmittance adjustment layer. The same measurement was performed in Examples 2 to 5 and Comparative Examples 1 to 3. The thicknesses of the spectral transmittance adjusting layer and the overcoat layer were measured in the same manner as in Example 1.

[0199] <Example 2> In Example 2, the solid content of the polyfunctional monomer and the acrylic polymer (1) An optical film was obtained in the same manner as in Example 1, except that the mass ratio was 67:33.

[0200] <Example 3> In Example 3, the solid content of the polyfunctional monomer and the acrylic polymer (1) An optical film was obtained in the same manner as in Example 1, except that the mass ratio was 50:50.

[0201] <Example 4> In Example 4, the same structure as in Example 1 was used except that the thickness of the spectral transmittance adjusting layer was 2 μm. An optical film was obtained in the same manner.

[0202] <Example 5> (Preparation of Spectral Transmittance Adjusting Layer Composition 2) Polyester resin (product name "Vylon 24SS", manufactured by Toyobo Co., Ltd.) with 25% solids The resin composition was then diluted with methyl ethyl ketone to prepare a resin composition. A polymerization initiator (Omnira manufactured by IGM Resins BV) was added to 120 parts by mass of the product. 4 parts by mass of D184 and Omnirad819 (mass ratio 50:50) and an indole compound (Product name: BONASORB UA-3912, manufactured by Orient Chemical Industries Co., Ltd.) 3 parts by mass, and a benzotriazole compound (product name "JF-79", Johoku Chemical Co., Ltd. 5 parts by weight of a leveling agent (product name "F568", manufactured by DIC Corporation) and 0.2 parts by weight of a leveling agent (product name "F568", manufactured by DIC Corporation). The above was mixed and thoroughly stirred to prepare a composition 2 for a spectral transmittance adjusting layer.

[0203] (Optical film manufacturing) The obtained composition 2 for the spectral transmittance adjusting layer was measured using a Maya bar to measure The surface of the triacetyl cellulose substrate was coated with a 25 μm thick film (A4 size). The coating film was then dried at 50° C. with a flow rate of 0.5 m / s. By circulating air for 30 seconds, the solvent in the coating is evaporated, and the UV light is applied for 50 minutes. mJ / cm 2 The coating is then cured by irradiating it so that the film thickness becomes 5 μm. A transmittance adjustment layer was formed on the triacetyl cellulose substrate. An optical film having a light-transmitting functional layer consisting only of a transmittance adjusting layer (SA layer) was obtained.

[0204] <Comparative Example 1> In Comparative Example 1, the solid content of the polyfunctional monomer and the acrylic polymer (1) was An optical film was obtained in the same manner as in Example 1, except that the mass ratio was 90:10.

[0205] <Comparative Example 2> (Preparation of Spectral Transmittance Adjusting Layer Composition 3) Multifunctional monomer (product name "KAYARAD PET-30", manufactured by Nippon Kayaku Co., Ltd.) Solvents: methyl ethyl ketone and methyl isobutyl ketone, weight ratio 50: The resin composition was then diluted with 50% water to prepare a resin composition. The polymerization initiators (Omnirad184 and Om 4 parts by mass of nirad819 (mass ratio 50:50) and an indole compound (Orient Chemical 3 parts by weight of "BONASORB UA-3912" manufactured by BONASORB Industrial Co., Ltd., and Rebellin Mix with 0.2 parts of a binder (product name "F568", manufactured by DIC Corporation) and stir well. In this way, a composition 3 for a spectral transmittance adjusting layer was prepared.

[0206] (Optical film manufacturing) A test piece was prepared in the same manner as in Example 5, except that the obtained composition 3 for a spectral transmittance adjusting layer was used. A 5μm thick spectral transmittance adjustment layer (SA layer) is formed on a triacetyl cellulose substrate. An optical film having a transmissive functional layer was obtained.

[0207] <Comparative Example 3> (Preparation of Spectral Transmittance Adjusting Layer Composition 4) Multifunctional monomer (product name "KAYARAD PET-30", manufactured by Nippon Kayaku Co., Ltd.) Solvents: methyl ethyl ketone and methyl isobutyl ketone, weight ratio 50: The resin composition was then diluted with 50% water to prepare a resin composition. The polymerization initiators (Omnirad184 and Om 4 parts by mass of nirad819 (mass ratio 50:50) and a benzotriazole compound (product name "JF-79" (manufactured by Johoku Chemical Co., Ltd.) 7 parts by mass, leveling agent (product name "F568" (manufactured by DIC Corporation) and 0.2 parts by mass of the mixture, and the spectral transmittance was adjusted by stirring thoroughly. Layer-styling composition 4 was prepared.

[0208] (Optical film manufacturing) The obtained composition 4 for the spectral transmittance adjusting layer was measured using a Maya bar to measure The surface of the triacetyl cellulose substrate was coated with a 25 μm thick film (A4 size). The coating film was then dried at 50° C. with a flow rate of 0.5 m / s. By passing air through the coating for 30 seconds, the solvent in the coating is evaporated, and the UV light is then turned on for 20 seconds. 0mJ / cm 2 The coating is then cured by irradiating it to a thickness of 8 μm. A transmittance adjusting layer was formed on the triacetyl cellulose substrate. An optical film having a light-transmitting functional layer consisting only of a light transmittance adjusting layer (SA layer) was obtained.

[0209] <Spectral transmittance> In the optical films according to the examples and comparative examples, the wavelengths were 380 nm, 410 nm, and 42 The spectral transmittance was measured at 0 nm and 440 nm. A spectrophotometer capable of measuring the transmittance of optical films cut to a size of 1.5 mm in 0.5% increments. Total (product name: UV-2450, manufactured by Shimadzu Corporation, light source: tungsten lamp and The optical film was placed in a 300-kV IR ... The film must be free of defects (contamination of foreign matter), cracks, wrinkles, and stains. The specimen was held in the spectrophotometer in a flat, curl-free state. Under these conditions, the wavelengths of 380 nm, 410 nm, 420 nm and 440 nm were The transmittance is measured at least five points within 1 nm after the measurement, and the average value is calculated. The spectral transmittance was measured at wavelengths of 380 nm, 410 nm, 420 nm, and 440 nm. The spectral transmittance at wavelengths of 380 nm, 410 nm, 420 nm and 440 nm is 3 The arithmetic mean value of the values ​​obtained by measuring three times is shown in FIG. Graphs showing the spectral transmittance for Nos. 1 to 3 are shown. (Measurement conditions) ·Wavelength range: 300nm~780nm Scan speed: Fast Slit width: 2.0 Sampling interval: Auto (0.5 nm interval) ·Lighting:C Light source: D2 and WI ·Field of view: 2° Light source switching wavelength: 360 nm S / R Switching: Standard Detector: PM Autozero: Performed at 550 nm after baseline scan

[0210] <Blue light blocking rate> The blue light blocking rate (BL blocking rate) of the optical films according to the examples and the comparative examples was measured. Specifically, we first set a 50mm x 50mm square plate in accordance with JIS T7333:2005. The transmittance of optical film cut into mm size can be measured in 0.5% increments using a spectrophotometer. UV meter (product name: UV-2450, manufactured by Shimadzu Corporation, light source: tungsten lamp and The optical film was placed in a 300-millimeter-long tube (100-millimeter-long tube and deuterium lamp) so that the substrate side of the optical film was the light source side. The film is free of defects (contamination of foreign matter), cracks, wrinkles, and dirt. The paper was also held in a flat, curl-free state in the spectrophotometer. Measure the transmittance at least 5 points within 1 nm before and after each wavelength from 500 nm to 495 nm. The average value was calculated to determine the spectral transmittance in the wavelength range of 380 nm to 495 nm. The blue light blocking rate (%) is A, and the average transmittance from 380 nm to 495 nm is B. The value (%) was taken as B, and the blue light blocking rate was calculated using the following formula. The spectral transmittance was measured three times and the arithmetic average value was used. The measurement conditions for the spectral transmittance were as follows: The same conditions for measuring the spectral transmittance at wavelengths of 380 nm, 410 nm, and 440 nm were used as above. It was as follows. A=100-B

[0211] <Yellow Index (YI), color coordinate a * and color coordinate b * > Yellow index and color coordinate a of the optical films according to the examples and comparative examples * and color Coordinate b * Specifically, the optical fiber was cut to a size of 50 mm x 50 mm. The film was then measured using a spectrophotometer (product name: UV-2450, manufactured by Shimadzu Corporation, light source: The optical film is placed in a 2000W lamp (200W for 1000W and 200W for 1000W) with the substrate side facing the light source. The optical film is free of defects (contamination of foreign matter), cracks, wrinkles, and dirt. The specimens were free of scratches and were held flat and curl-free in the spectrophotometer. The transmittance was measured at wavelengths of 300 nm to 780 nm. On the monitor, read the transmittance measurement data and enter "YI" and "a * " and "b * By checking "YI, a * and b * We obtained the wavelength The measurement conditions for the transmittance from 300 nm to 780 nm are the above wavelengths of 380 nm, 410 nm, and The measurement conditions for the spectral transmittance at 440 nm and 450 nm were the same as those for the measurement of the spectral transmittance at 440 nm and 450 nm.

[0212] <Spectral transmittance gradient at wavelengths of 410nm to 420nm> In the optical films according to the examples and the comparative examples, Specifically, the slope of the spectral transmittance of a light beam cut into a size of 50 mm x 50 mm was calculated. A spectrophotometer (product name: UV-245) that can measure the transmittance of optical films in 0.5% increments 0, manufactured by Shimadzu Corporation, light source: tungsten lamp and deuterium lamp) The substrate side of the film was placed on the light source side. The optical film has defects (contamination of foreign matter) It is free of scratches, cracks, wrinkles, stains, and curls. In this state, the sample was held in the spectrophotometer at wavelengths of 410 nm to 420 nm. The transmittance was measured at least five points within 1 nm before and after each measurement, and the average value was calculated. The spectral transmittance at wavelengths of 410 nm to 420 nm was then calculated. Using the light transmittance, the slope of the spectral transmittance from 410 nm to 420 nm was calculated by the least squares method. The slope was calculated as the arithmetic mean value of three measurements. The measurement conditions are the spectral transmittance at the wavelengths of 380 nm, 410 nm, and 440 nm. The measurement conditions were the same as those in .

[0213] <Indentation hardness> Indentation of the spectral transmittance adjusting layer in the optical films according to the examples and comparative examples The indentation hardness was measured using a HYSITRON (hygitron) The measurements were carried out using a "TI950 TriboIndenter" manufactured by TI. First, the optical film was cut to a size of 1 mm x 10 mm and embedded in embedding resin. A test sample suitable for hardness measurement using the nanoindentation method was prepared. The measurement samples were prepared using the Ultramicrotome EM UC7 (Leica Microtome). Next, a scanning electron microscope (SEM) was used to measure the cross section of the sample. Observation with a scanning electron microscope (SEM) revealed that the interface line between the spectral transmittance adjustment layer and the overcoat layer It was confirmed whether the surface of the measurement sample to be pressed with the indenter was clearly observed. The measurement sample is placed on the HYSITRON T The sample was fixed on the stage of an I950 TriboIndenter and observed by SEM. In the case where the interface line between the spectral transmittance adjusting layer and the overcoat layer is clearly observed, The spectral transmittance adjusting layer and the overcoat layer are disposed on the flat central portion of the spectral transmittance adjusting layer. If the interface line is not clearly observed, the light-transmitting functional layer is The Berkovich-type indenter was used in a load-control system so that the maximum indentation load was 300 μN. The specimen is pressed into the measurement position at a speed of 10 nm / s, then held at the maximum load for 5 seconds, and then pressed down at the same speed. The indentation depth h corresponding to the indentation load F (μN) at this time was (nm) was continuously measured, and a load-displacement curve was created. From the load-displacement curve, Maximum pressing load F max (N) is the projected area A where the indenter and the spectral transmittance adjustment layer are in contact p (mm 2 The value was calculated by dividing the above by A p The indenter tip curvature was corrected using the standard method. The indentation hardness was measured at 10 points. The arithmetic mean value was calculated.

[0214] <Flexibility> In the examples and comparative examples, the following was performed in accordance with JIS K5600-5-1:1999: A bending test was performed to evaluate the bending property. The cut optical film was attached to a stainless steel rod with a diameter of 2 mm, with the light-transmitting functional layer on the outside. The optical film was then wrapped around the substrate so that both ends in the long side direction of the optical film faced each other. In this state, the substrate was kept for 5 seconds. After the optical film was held in place, the optical film was released, and the short side of the optical film that had been in contact with the stainless steel rod was We checked whether any cracks had occurred. We also checked whether the light-transmitting functional layer was on the inside. A mandrel test was performed under the same conditions as above, and the optical film in contact with the stainless steel rod was shortened. It was checked whether cracks had occurred in the side direction. The evaluation results were as follows. ○: No cracks were found in the optical film in any of the mandrel tests. . ×: Cracks were observed in the optical film in any of the mandrel tests.

[0215] <Display panel degradation evaluation> The optical films according to the examples and comparative examples were used for organic light-emitting diode (OLED) panels. ) to conduct light resistance tests on samples placed on the OLED panel to see if it deteriorates. Specifically, the sample was an optical fiber cut to a size of 50 mm x 50 mm. Room and smartphones (product name "Galaxy S7", Samsung Elect The LED (manufactured by Ronics Co., Ltd.) should be placed on the OLED panel so that it faces downward. The sample OLED panel was then lit up to produce an optical filter. The brightness of the light emitted from the film is measured from the thickness direction of the optical film using a spectroradiometer (product name: The measurements were taken using a "CS2000" (manufactured by Konica Minolta) at a measurement angle of 1°. After that, the sample was tested using a light resistance tester (product name: "Ultraviolet Fade Meter U48AU" by Suga Test Co., Ltd.) The carbon arc lamp was placed in a test chamber (manufactured by Experimental Machinery Co., Ltd.) and placed under an environment of 42°C and 50% relative humidity. A light resistance test was conducted in which the surface of the optical film was irradiated with light from a filter for 50 hours. Take the sample out of the light resistance tester and light the OLED panel of the sample after the light resistance test. The luminance of the light emitted from the optical film is calculated from the thickness direction of the optical film as a function of the spectral radiation. Using a luminance meter (product name "CS2000", manufactured by Konica Minolta), at a measurement angle of 1° From these measured luminance values, the luminance after the heat resistance test was calculated based on the luminance before the heat resistance test. The luminance maintenance rate was calculated by dividing the luminance maintenance rate by the luminance maintenance rate A from the sample before the heat resistance test. The brightness of the light emitted from the sample after the heat resistance test is B, and the brightness of the light emitted from the sample after the heat resistance test is C. It was calculated using the formula: A=C / B×100 The obtained brightness maintenance rate is used to determine whether the OLED panel has deteriorated during the light resistance test. Specifically, if the brightness maintenance rate is less than 80%, the OLED panel is deemed inferior. If the brightness maintenance rate is 80% or more, the OLED panel is not degraded. The evaluation criteria were as follows: No degradation of the OLED panel was observed. ×: Deterioration of the OLED panel was confirmed.

[0216] The results are shown in Tables 1 and 2 below. [Table 1]

[0217] [Table 2]

[0218] As shown in Table 1, in the optical films according to Comparative Examples 1 to 3, the wavelength of 380 nm The spectral transmittance at a wavelength of 410 nm is less than 1%, and the spectral transmittance at a wavelength of 410 nm is 10% or more. The requirement is that the spectral transmittance at a wavelength of 440 nm is 70% or more and that the transmittance is less than 60%. Since the condition was not met, even though it was thin, the blue light blocking rate was low. The optical film showed poor yellowing and / or the yellowing was not suppressed. The type and ratio of the spectral transmittance adjuster to be added is important because it is affected by the range of wavelengths to be measured. For this reason, the optical films according to Comparative Examples 1 and 3 are In the case of 410nm, the YI was low, but the spectral transmittance was high and the blue light blocking rate was In order to reduce YI, the spectral curve must have a sharp rise in the visible light range. It is preferable that the slope of the spectral transmittance at wavelengths of 410 nm to 420 nm is high. In the optical film according to Comparative Example 2, the spectral transmittance at wavelengths of 410 nm to 420 nm It is believed that the YI was high because the rate slope was small.

[0219] In contrast, in the optical films according to Examples 1 to 5, the distribution at a wavelength of 380 nm was Light transmittance is less than 1%, and the spectral transmittance at a wavelength of 410 nm is 10% or more and less than 60%. and meets the requirement that the spectral transmittance at a wavelength of 440 nm is 70% or more. So, it is thin, has excellent blue light blocking (shielding) rate, and has optical filter. The yellowish color of the gel was suppressed. [Explanation of symbols]

[0220] 10, 20, 30, 40, 50...Optical film 11...Light-transmitting base material 12, 21, 31, 41, 51...light-transparent functional layer 13, 32, 42, 52...Spectral transmittance adjustment layer 14...Overcoat layer 33...Vapour-deposited layer 43…Invisible Layer 43A…High refractive index layer 43B…Low refractive index layer 50...Polarizing plate 51...Polarizer 60...Image display device 70...Display panel 71...Display element

Claims

1. An optical film comprising a light-transmitting substrate and a light-transmitting functional layer provided on one surface of the light-transmitting substrate, The spectral transmittance at a wavelength of 380 nm is less than 1%, The spectral transmittance at a wavelength of 410 nm is more than 10% and less than 60%, The spectral transmittance at a wavelength of 440 nm is 70% or more, the light-transmitting substrate contains a light-transmitting resin, The thickness of the light-transmitting functional layer is 9 μm or less, The optical film, wherein the light-transmitting functional layer does not contain a fluorescent whitening agent.

2. The optical film according to claim 1 , wherein the optical film has a yellow index of 1 or more and 12 or less.

3. The optical film according to claim 1 , wherein the optical film has a blue light blocking rate of 30% or more.

4. 4. The optical film according to claim 1, wherein a slope of the transmission spectrum in the wavelength range of 410 nm to 420 nm obtained by the least squares method is 2 or more.

5. The optical film according to claim 1 , wherein the light-transmitting functional layer comprises a spectral transmittance adjusting layer containing a resin and a spectral transmittance adjusting agent.

6. The optical film according to claim 1 , A polarizer provided on one surface side of the optical film; A polarizing plate comprising:

7. A display element; The optical film according to claim 1 or the polarizing plate according to claim 6, which is disposed on a viewer side relative to the display element; An image display device comprising:

8. The image display device according to claim 7 , wherein the display element is an organic light-emitting diode display element.

Citation Information

Patent Citations

  • Ultraviolet-absorbing transparent material

    JP1994145387A

  • Polarizing plate with reflection preventing layer

    JP1998062622A

  • Optical filter

    JP2011164286A

  • Functional film

    JP2014164111A

  • Optical film, polarizing plate using the same, touch panel, display member, and display device

    JP2017003884A