Niobate particles, method for producing niobate particles, resin composition and molded product
A controlled crystal growth method for niobate particles using a flux process enhances their piezoelectric performance by achieving larger crystallite sizes and uniform shapes, addressing the limitations of existing production techniques.
Patent Information
- Application Number
- JP2024504939
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-04-21
- Filing Date
- 2023-04-19
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2043-04-19
AI Technical Summary
Existing methods for producing niobate particles do not effectively control crystal growth, limiting the versatility and performance of resulting niobate particles, particularly in piezoelectric applications where larger crystallite sizes are desired.
The production method involves calcining a niobium compound and a tantalum compound in the presence of potassium and/or sodium compounds, with optional molybdenum compounds, to achieve niobate particles with a controlled average crystallite size of 80 nm or more and a perovskite structure, using a flux method to promote crystal growth.
The method produces niobate particles with enhanced crystal growth, resulting in improved piezoelectric performance and efficiency, as demonstrated by higher crystallite sizes and uniform particle shapes, suitable for applications in piezoelectric bodies and other uses.
Smart Images

Figure 0007571914000006 
Figure 0007571914000007 
Figure 0007571914000008
Abstract
Description
[Technical field]
[0001] The present invention relates to niobate particles, a method for producing niobate particles, a resin composition, and a molded article. This application claims priority based on Japanese Patent Application No. 2022-070229, filed in Japan on April 21, 2022, the contents of which are incorporated herein by reference. [Background technology]
[0002] Alkali metal niobates are widely used as piezoelectric materials, fillers, catalysts, water purification materials, and the like.
[0003] An example of Patent Document 1 shows a method for producing sodium potassium niobate particles, in which Na2CO3, K2CO3, and Nb2O5 are used as raw material powders, and the mixture of the raw material powders is sintered at 1100°C for 2 hours and then crushed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2020-145408 A Summary of the Invention [Problem to be solved by the invention]
[0005] Controlling the crystal growth of niobate particles is a very important technique for increasing the versatility of applications for the resulting niobate particles. x Na (1-x) NbO3 (0≦x≦1) has a perovskite structure and can be used, for example, as a piezoelectric material. As a piezoelectric material, it is expected that the larger the crystallite size, the better the piezoelectric effect will be. However, there is still room for improvement in the crystal growth of niobate particles obtained by conventional methods for producing niobate particles.
[0006] The present invention has been made to solve the above problems, and an object thereof is to provide niobate particles excellent in the degree of crystal growth.
Means for Solving the Problems
[0007] The present invention has the following aspects.
[0008] (1) K x Na (1-x) Nb y Ta (1-y) O3 (where 0 ≦ x ≦ 1 and 0 < y ≦ 1), and the niobate particles include a crystal structure of niobate represented by the crystal structure is such that the average crystallite size determined from the peak of the niobate at 2θ = 23.0 ± 1.0° obtained by X-ray diffraction measurement is 80 nm or more. (2) The niobate particles according to (1) above, wherein the crystal structure includes a perovskite crystal structure. (3) The niobate particles according to (1) or (2) above, having a cubic shape. (4) The niobate particles according to any one of (1) to (3) above, wherein the crystal structure is such that the average crystallite size determined from the peak of the niobate at 2θ = 32.0 ± 1.2° obtained by X-ray diffraction measurement is 50 nm or more. (5) The niobate particles according to any one of (1) to (4) above, wherein the median diameter D calculated by the laser diffraction / scattering method 50 is 0.1 to 100 μm. (6) The niobate particles according to any one of (1) to (5) above, wherein the ratio (R) of the peak intensity I(100) of the peak of the niobate at 2θ = 23.0 ± 1.0° obtained by X-ray diffraction measurement to the peak intensity I(110) of the peak at 2θ = 32.0 ± 1.2° is 1 or more. R = I(100) / I(110) (7) The niobate particles according to any one of (1) to (6), wherein the total content of niobium, or niobium and tantalum, in the niobate particles is 50 to 99 mass% in terms of Nb2O5 and Ta2O5, relative to 100 mass% of the total mass of the niobate particles, as determined by XRF analysis of the niobate particles. (8) The niobate particles according to any one of (1) to (7), wherein the potassium and / or sodium content in the niobate particles is determined by XRF analysis of the niobate particles, and the total content in terms of K2O and Na2O is 0.5 to 40 mass% relative to 100 mass% of the total mass of the niobate particles. (9) The niobate particles according to any one of (1) to (8) above, which contain molybdenum. (10) The niobate particles according to (9), wherein the molybdenum content in the niobate particles is determined by XRF analysis of the niobate particles, and the content in terms of MoO3 is 0.01 to 20 mass% with respect to 100 mass% of the total mass of the niobate particles. (11) A method for producing niobate particles according to any one of (1) to (10), comprising the steps of: A method for producing niobate particles, comprising calcining a niobium compound, or a niobium compound and a tantalum compound, in the presence of a potassium compound and / or a sodium compound. (12) The method for producing niobate particles according to (11) above, wherein the sodium compound is sodium carbonate and the potassium compound is potassium carbonate. (13) A method for producing niobate particles according to (11) or (12) above, comprising calcining a niobium compound, or a niobium compound and a tantalum compound, in the presence of a molybdenum compound and a potassium compound and / or a sodium compound. (14) The method for producing niobate particles according to (13) above, wherein the molybdenum compound is at least one compound selected from the group consisting of molybdenum trioxide, potassium molybdate, and sodium molybdate. (15) The method includes a step of mixing a niobium compound or a niobium compound and a tantalum compound with a potassium compound and / or a sodium compound to obtain a mixture, and a step of calcining the mixture, The method for producing niobate particles according to any one of (11) to (14), wherein a molar ratio (K+Na) / (Nb+Ta) of potassium atoms and sodium atoms to niobium atoms and tantalum atoms in the mixture is 1.1 or more. (16) A resin composition comprising the niobate particles according to any one of (1) to (10) above and a resin. (17) A molded article obtained by molding the resin composition according to (16) above. Effect of the Invention
[0009] According to the present invention, it is possible to provide niobate particles having an excellent degree of crystal growth. The present invention also provides a method for producing the niobate particles. Furthermore, according to the present invention, there can be provided a resin composition containing the niobate particles, and a molded article thereof. [Brief description of the drawings]
[0010] [Figure 1] 1 is a SEM image of KxNa(1-x)NbO3 particles of Example 1. [Diagram 2] 1 is a SEM image of KxNa(1-x)NbO3 particles of Example 2. [Diagram 3] 1 is a SEM image of KxNa(1-x)NbO3 particles of Example 3. [Figure 4] 1 is a SEM image of KxNa(1-x)NbO3 particles of Example 4. [Diagram 5] 1 is a SEM image of KxNa(1-x)NbO3 particles of Example 5. [Figure 6] 1 is a SEM image of NaNbO3 particles of Example 6. [Figure 7] 1 is a SEM image of KNbO3 particles of Example 7. [Figure 8]1 is a SEM image of KxNa(1-x)NbyTa(1-y)O3 particles of Example 8. [Figure 9] 1 is a SEM image of KxNa(1-x)NbyTa(1-y)O3 particles of Example 9. [Figure 10] 1 is a SEM image of KxNa(1-x)NbyTa(1-y)O3 particles of Example 10. [Figure 11] 1 is a SEM image of KxNa(1-x)NbyTa(1-y)O3 particles of Example 11. [Figure 12] 1 is a SEM image of KxNa(1-x)NbyTa(1-y)O3 particles of Example 12. [Figure 13] 1 is a SEM image of KxNa(1-x)NbyTa(1-y)O3 particles of Example 13. [Figure 14] 1 is an SEM image of KxNa(1-x)NbO3 particles of Comparative Example 1. [Figure 15] 1 shows X-ray diffraction (XRD) patterns of powder samples of Examples 1 to 5. [Figure 16] 1 shows X-ray diffraction (XRD) patterns of powder samples of Examples 6 to 7. [Figure 17] 1 shows X-ray diffraction (XRD) patterns of powder samples of Examples 8 to 12. [Figure 18] 1 is an X-ray diffraction (XRD) pattern of a powder sample of Example 13. [Figure 19] 1 is an X-ray diffraction (XRD) pattern of a powder sample of Comparative Example 1. [Figure 20] FIG. 2 is a schematic diagram showing the configuration of a speaker used for evaluating piezoelectric performance in the examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, embodiments of the niobate particles, the method for producing the niobate particles, the resin composition, and the molded article of the present invention will be described.
[0012] <Niobate particles> The niobate particles of the embodiment include K x Na (1-x) Nby Ta (1-y) It includes the crystal structure of a niobate represented by O3 (where 0 ≦ x ≦ 1 and 0 < y ≦ 1), and the average crystallite size obtained from the peak of the niobate at 2θ = 23.0 ± 1.0° obtained by X-ray diffraction measurement is 80 nm or more.
[0013] The niobate particles of the embodiment are K x Na (1-x) Nb y Ta (1-y) It contains a niobate compound represented by O3. In the formula K x Na (1-x) Nb y Ta (1-y) In O3, x is 0 ≦ x ≦ 1 and y is 0 < y ≦ 1. When x is 0 < x < 1 and y is 0 < y < 1, K x Na (1-x) Nb y Ta (1- y) O3 is potassium sodium tantalum niobate. When x = 0 and y is 0 < y < 1, K x Na (1-x) Nb y Ta (1-y) O3 is sodium tantalum niobate (NaNb y Ta (1-y) O3). When x = 1 and y is 0 < y < 1, K x Na (1-x) Nb y Ta (1-y) O3 is potassium tantalum niobate (KNb y Ta (1-y) O3). When x is 0 < x < 1 and y = 1, K x Na (1-x) Nb y Ta (1-y) O3 is potassium sodium niobate (K x Na (1-x) NbO3). When x = 0 and y = 1, K x Na (1-x) Nb yTa (1-y) O3 is sodium niobate (NaNbO3). When x = 1 and y = 1, K x Na (1-x) Nb y Ta (1-y) O3 is potassium niobate (KNbO3).
[0014] It is known that it is preferably characteristic for the piezoelectric material to include a composition called a morphotropic phase boundary (MPB) at the boundary between different crystal systems (such as monoclinic and orthorhombic, orthorhombic and tetragonal). The values of x and y can be adjusted so as to be a composition near this phase boundary. K x Na (1-x) Nb y Ta (1-y) In KTaNaNbO3, for example, it is preferable that 0.4 ≦ x ≦ 0.6, and more preferably 0.45 ≦ x ≦ 0.55. K x Na (1-x) Nb y Ta (1-y) In KTaNaNbO3, for example, it is preferable that 0.5 ≦ y ≦ 1. Note that, for improving characteristics other than piezoelectric performance such as durability, it is possible to include a composition outside the MPB composition itself. Therefore, the composition of the niobate particles of the embodiment is not limited to this preferable range, and is effective in the entire range of 0 ≦ x ≦ 1 and 0 < y ≦ 1.
[0015] Also, for the purpose of suppressing leakage current and maintaining insulation, elements having a valence lower than that of Nb, such as elements such as Mn, Cr, Co, Ni, and Zn, may be appropriately included within a range of several moles (1 to 3 mol%) with respect to Nb. Further, as inevitable impurities in the raw materials, elements such as Fe may be included.
[0016] In this specification, the numerical values of x and y are K in any of the above cases x Na (1- x) Nb y Ta (1-y)Even if the particles contain O3, they may be simply called "niobate particles." In addition, the numerical ranges of x and y may be omitted.
[0017] The type, composition, and crystal structure of the niobate contained in the niobate particles of the embodiment can be identified by the XRD pattern of the spectrum obtained by XRD analysis.
[0018] The average crystallite size of the crystal structure contained in the niobate particles of the embodiment can be determined by the following measurement method.
[0019] [Crystallite size measurement] Measurements are performed using an X-ray diffraction apparatus (e.g., SmartLab, manufactured by Rigaku Corporation), a high intensity, high resolution crystal analyzer (CALSA) as a detector, and analysis software. The measurement method is the 2θ / θ method, and the average crystallite size is calculated using the Scherrer formula from the half-width of the target peak (a peak having a peak top in the target 2θ range). The measurement conditions are a scan speed of 0.05 degrees / min, a scan range of 20 to 70 degrees, a step of 0.002 degrees, and a standard width of the device of 0.028° (Si).
[0020] The crystal structure contained in the niobate particles of the embodiment has an average crystallite size determined from the peak at 2θ=23.0±1.0° of 80 nm or more, preferably 90 nm or more, and more preferably 100 nm or more. When the average crystallite size of the niobate particles is equal to or greater than the above lower limit, excellent piezoelectric performance is exhibited.
[0021] The upper limit of the average crystallite size of the crystal structure contained in the niobate particles of the embodiment, calculated from the peak at 2θ=23.0±1.0°, is not particularly limited, but may be 1000 nm or less, 800 nm or less, or 500 nm or less.
[0022] An example of the above-mentioned numerical range of the average crystallite size calculated from the peak at 2θ=23.0±1.0° of the crystal structure contained in the niobate particles of the embodiment may be 80 nm or more and 1000 nm or less, 90 nm or more and 800 nm or less, or 100 nm or more and 500 nm or less.
[0023] K x Na (1-x) Nb y Ta (1-y) Depending on the composition, O3 may exhibit a crystal system different from monoclinic, orthorhombic, or tetragonal, and the assignment of the faces differs depending on the crystal system. Unless otherwise specified in this specification, the notation of the face index is based on the assumption that the crystal structure is a cubic system.
[0024] For the target peaks obtained by the above crystallite size measurement, if the peaks are assigned assuming a cubic crystal system without considering peak splitting, the above peak at 2θ=23.0±1.0° corresponds to the (100) plane of the cubic crystal system. If the peaks are split, the crystallite size is defined by the peak with the strongest intensity.
[0025] The average crystallite size of the crystal structure contained in the niobate particles of the embodiment, as determined from the peak at 2θ=32.0±1.2°, is preferably 50 nm or more, more preferably 80 nm or more, and even more preferably 100 nm or more. When the average crystallite size of the niobate particles is equal to or greater than the above lower limit, even more excellent piezoelectric performance is exhibited.
[0026] The upper limit of the average crystallite size of the crystal structure contained in the niobate particles of the embodiment, calculated from the peak at 2θ=32.0±1.2°, is not particularly limited, but may be 1000 nm or less, 800 nm or less, or 700 nm or less.
[0027] An example of the above-mentioned numerical range of the average crystallite size calculated from the peak at 2θ=32.0±1.2° of the crystal structure contained in the niobate particles of the embodiment may be 50 nm or more and 1000 nm or less, 80 nm or more and 800 nm or less, or 100 nm or more and 700 nm or less.
[0028] For the target peaks obtained by the above crystallite size measurement, if the peaks are assigned assuming a cubic crystal system without considering peak splitting, the above peak at 2θ=32.0±1.2° corresponds to the (110) plane of the cubic crystal system. If the peaks are split, the crystallite size is defined by the peak with the strongest intensity.
[0029] The crystal structure of the niobate particles of the embodiment has an average crystallite size, determined from the peak at 2θ=57.0±1.0°, of preferably 15 nm or more, more preferably 20 nm or more, and even more preferably 30 nm or more. When the average crystallite size of the niobate particles is equal to or greater than the above lower limit, even more excellent piezoelectric performance is exhibited.
[0030] The upper limit of the average crystallite size of the crystal structure contained in the niobate particles of the embodiment, calculated from the peak at 2θ=57.0±1.0°, is not particularly limited, but may be 500 nm or less, 400 nm or less, or 300 nm or less.
[0031] An example of the above numerical range of the average crystallite size calculated from the peak at 2θ=57.0±1.0° of the crystal structure contained in the niobate particles of the embodiment may be 15 nm or more and 500 nm or less, 20 nm or more and 400 nm or less, or 30 nm or more and 300 nm or less.
[0032] For the target peak obtained by the above crystallite size measurement, if the peak is assigned assuming a cubic crystal system without considering peak splitting, the above peak at 2θ=57.0±1.0° corresponds to the (211) plane of the cubic crystal system. If the target peak is split, the crystallite size is defined by the peak with the strongest intensity.
[0033] According to the manufacturing method of the embodiment described below, the crystal growth of the produced niobate particles can be well controlled, and niobate particles with an improved average crystallite size can be easily obtained.
[0034] The average crystallite size can be controlled by the amount and type of flux used and the firing conditions in the production method described below.
[0035] The crystal structure of the niobate particles of embodiments may include a perovskite crystal structure.
[0036] The niobate particles of embodiments can have a cubic shape.
[0037] In this specification, the term "cubic" refers to a shape derived from a perovskite structure, and preferably has a substantially cubic hexahedral shape, and each face constituting the hexahedron may be flat or may be curved or uneven.
[0038] For each of the peaks shown above obtained by X-ray diffraction measurement, the ratio (R) of the peak intensity I(100) of the peak having its top at 2θ=23.0±1.0° to the peak intensity I(110) of the peak having its top at 2θ=32.0±1.2° can be calculated. R = I(100) / I(110) The peak intensity is the value at the peak top of the peak.
[0039] The value of R in the niobate particles of the embodiment is preferably 1 or more, more preferably 1.1 or more, even more preferably 2 or more, and particularly preferably 3 or more.
[0040] When the diffraction of I(100) with a peak top at 2θ=23.0±1.0° is measured strongly, that is, when the value of R is 1 or more, it is considered to indicate that the particles in the sample being measured are arranged with the direction of one face of the hexahedron corresponding to the (100) face aligned. This is considered to occur more easily when the particle shape is more regular. That is, the niobate particles of the embodiment in which the value of R is 1 or more are of high quality and have a regular particle shape. The niobate particles according to the embodiment in which the value of R is 1 or more have excellent filling properties when made into a resin composition described below.
[0041] According to a manufacturing method of an embodiment described later, it is possible to manufacture niobate particles having a perovskite crystal structure and a cubic shape.
[0042] A higher firing temperature tends to result in niobate particles with a larger average crystallite size and larger particle size.
[0043] When the niobate particles have a cubic shape, the particle size is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more. When the niobate particles have a cubic shape, the upper limit of the particle size is not particularly limited, but may be, for example, 100 μm or less, 80 μm or less, or 50 μm or less. When the niobate particles have a cubic shape, the upper limit numerical range of the particle size may be, for example, 0.1 to 100 μm, 0.5 to 80 μm, or 1 to 50 μm.
[0044] In this specification, the "particle size" of a niobate particle having a cubic shape refers to the length of one side of a hexahedron determined from a particle image of a primary particle of the niobate particle in a two-dimensional image taken with a scanning electron microscope (SEM). The particle size value of the cubic shaped niobate is the average value obtained from 50 or more niobate particles randomly selected from the idiomorphic particles to be measured.
[0045] When niobate particles having a cubic shape are included, it is preferable that 50% or more of the particles have a cubic shape by mass or number, more preferably 80% or more of the particles have a cubic shape, and even more preferably 90% or more of the particles have a cubic shape.
[0046] The median diameter D of the niobate particles of the embodiment calculated by a laser diffraction / scattering method 50 The thickness may be 0.1 to 100 μm, may be 0.5 to 80 μm, or may be 1 to 50 μm.
[0047] D calculated by a laser diffraction / scattering method for the niobate particles of the embodiment 10 The thickness may be 0.05 to 70 μm, may be 0.1 to 50 μm, or may be 0.5 to 20 μm.
[0048] The median diameter D of the niobate particles of the embodiment calculated by a laser diffraction / scattering method 90 The thickness may be 0.5 to 150 μm, may be 1 to 100 μm, or may be 3 to 70 μm.
[0049] The median diameter D of a niobate particle sample calculated by the laser diffraction / scattering method 50 D can be calculated as the particle size at which the volume cumulative percentage is 50% in the particle size distribution measured in a dry state using a laser diffraction particle size distribution analyzer. 10can be determined as the particle diameter at the point where the distribution curve of the volume integration % intersects the horizontal axis at 10% from the small particle side, D 90 can be determined as the particle diameter at the point where the distribution curve of the volume integration % intersects the horizontal axis at 90% from the small particle side.
[0050] The specific surface area of the niobate particles of the embodiment, determined by the BET method, may be 0.02 to 20 m 2 / g, may be 0.04 to 10 m 2 / g, or may be 0.05 to 3 m 2 / g.
[0051] The above specific surface area is measured with a specific surface area meter (for example, BELSORP-mini manufactured by MicrotracBEL Corporation), and the surface area per 1 g of the sample measured from the adsorption amount of nitrogen gas by the BET method (Brunauer-Emmett-Teller method) is calculated as the specific surface area (m 2 / g).
[0052] The niobate particles of the embodiment contain K x Na (1-x) Nb y Ta (1-y) O3 (where 0 ≤ x ≤ 1, 0 < y ≤ 1).
[0053] The niobate particles of the embodiment preferably contain 65 mass% or more, more preferably 65 to 99.999 mass%, still more preferably 70 to 99.97 mass%, and even more preferably 75 to 99.95 mass% of the K x Na (1-x) Nb y Ta (1-y) O3 with respect to 100 mass% of the niobate particles.
[0054] The niobate particles of the embodiment contain niobium and may further contain tantalum.
[0055] The niobium or the total content of niobium and tantalum in the niobate particles is determined by XRF analysis of the niobate particles, and the total content in terms of Nb2O5 and Ta2O5 relative to 100% by mass of the total mass of the niobate particles may be 50% by mass or more, 50 to 99% by mass, 60 to 98% by mass, or 70 to 95% by mass.
[0056] The total content in terms of Nb2O5 and Ta2O5 refers to the sum of the amount of Nb2O5 obtained by converting the niobium content determined by XRF analysis using a calibration curve in terms of Nb2O5, and the amount of Ta2O5 obtained by converting the tantalum content determined by XRF analysis using a calibration curve in terms of Ta2O5. x Na (1-x) Nb y Ta (1-y) When y=1 in O3, the tantalum content may be zero.
[0057] The niobate particles of an embodiment include potassium and / or sodium.
[0058] The potassium and / or sodium content in the niobate particles is determined by XRF analysis of the niobate particles, and the total content in terms of KO and NaO relative to 100% by mass of the total mass of the niobate particles may be 0.5% by mass or more, 0.5 to 40% by mass, 1 to 30% by mass, or 3 to 25% by mass.
[0059] The total content in terms of K2O and Na2O refers to the sum of the amount of K2O obtained by converting the potassium content determined by XRF analysis using a calibration curve in terms of K2O, and the amount of Na2O obtained by converting the sodium content determined by XRF analysis using a calibration curve in terms of Na2O. x Na (1-x) Nb y Ta (1-y)When x=0 or 1 in O3, the potassium content or sodium content may be 0.
[0060] The niobate particles of an embodiment may further include molybdenum.
[0061] The niobate particles of the embodiment may contain molybdenum derived from a molybdenum compound that may be used in the manufacturing method described below. In addition, the niobate particles of the embodiment can achieve highly efficient crystal growth by using a molybdenum compound in the manufacturing method described below.
[0062] The state and amount of molybdenum contained in the niobate particles of the embodiment are not particularly limited, and may be contained in the niobate particles as molybdenum metal, molybdenum oxide, a partially reduced molybdenum compound, etc. Molybdenum is considered to be contained in the niobate particles as MoO3, but may also be contained in the niobate particles as MoO2, MoO, etc. other than MoO3.
[0063] The form in which molybdenum is contained is not particularly limited, and may be contained in a form in which it is attached to the surface of the niobate particle, may be contained in a form in which it is substituted as part of the crystal structure of the niobate particle, may be contained in an amorphous state, or may be a combination of these.
[0064] When the niobate particles of the embodiment contain molybdenum, the molybdenum content, calculated as MoO3 relative to the total mass of the niobate particles (100 mass%), determined by XRF analysis of the niobate particles, may be 0.01 mass% or more, 0.01 to 20 mass%, 0.05 to 15 mass%, or 0.06 to 10 mass%.
[0065] The content in terms of MoO3 refers to the value obtained by converting the molybdenum content determined by XRF analysis into the amount of MoO3 using a calibration curve in terms of MoO3.
[0066] The above values of the molybdenum content, the total content of niobium and tantalum, and the total content of potassium and sodium can be freely combined.
[0067] An example of the niobate particles of the embodiment can be niobate particles having a molybdenum content of 0 to 20 mass% in terms of MoO3, a total content of niobium and tantalum in terms of Nb2O5 and Ta2O5 of 50 to 99 mass%, and a total content of potassium and sodium in terms of KO and Na2O of 0.5 to 40 mass%, relative to 100 mass% of the total mass of the niobate particles, as determined by XRF analysis of the niobate particles. Another example of the niobate particles of the embodiment can be niobate particles having a molybdenum content of 0.01 to 20 mass% in terms of MoO3, a total content of niobium and tantalum in terms of Nb2O5 and Ta2O5 of 50 to 99 mass%, and a total content of potassium and sodium in terms of KO and Na2O of 0.5 to 40 mass%, relative to 100 mass% of the total mass of the niobate particles, as determined by XRF analysis of the niobate particles. Another example of the niobate particles of the embodiment can be niobate particles having a molybdenum content of 0.05 to 15 mass% in terms of MoO3, a total content of niobium and tantalum in terms of Nb2O5 and Ta2O5 of 60 to 98 mass%, and a total content of potassium and sodium in terms of KO and Na2O of 1 to 30 mass%, relative to 100 mass% of the total mass of the niobate particles, as determined by XRF analysis of the niobate particles. Another example of the niobate particles of the embodiment can be niobate particles having a molybdenum content of 0.06 to 10 mass% in terms of MoO3, a total content of niobium and tantalum in terms of Nb2O5 and Ta2O5 of 70 to 95 mass%, and a total content of potassium and sodium in terms of KO and Na2O of 3 to 25 mass%, relative to 100 mass% of the total mass of the niobate particles, as determined by XRF analysis of the niobate particles.
[0068] The niobate particles of the embodiment can be provided as an aggregate of niobate particles. The above-mentioned crystallite size, particle size distribution, specific surface area, numerical values of x and y, molybdenum content, niobium content, tantalum content, potassium content, and sodium content can be values obtained by using the aggregate as a sample.
[0069] The niobate particles of the embodiment can be produced, for example, by the <<Production method of niobate particles>> described later. The niobate particles of the present invention are not limited to those produced by the method for producing niobate particles according to the following embodiment.
[0070] The niobate particles of the embodiment can be used as a piezoelectric material, a catalyst, a water purification material, and the like.
[0071] <Method for producing niobate particles> A method for producing niobate particles according to an embodiment includes calcining a niobium compound, or a niobium compound and a tantalum compound, in the presence of a potassium compound and / or a sodium compound.
[0072] According to the method for producing niobate particles of this embodiment, it is possible to produce the niobate particles according to the embodiment of the present invention described above.
[0073] Moreover, according to the method for producing niobate particles of the present embodiment, a niobium compound, or a niobium compound and a tantalum compound, are fired in the presence of a potassium compound and / or a sodium compound, so that the degree of crystal growth of the produced niobate particles is excellent. Furthermore, according to the method for producing niobate particles of the present embodiment, the niobium compound, or the niobium compound and the tantalum compound, are fired in the presence of potassium carbonate and / or sodium carbonate, thereby producing niobate particles with an excellent degree of crystal growth.
[0074] A preferred method for producing niobate particles can include a step of mixing a niobium compound, or a niobium compound and a tantalum compound, with a potassium compound and / or a sodium compound to form a mixture (mixing step), and a step of calcining the mixture (calcining step).
[0075] In the method for producing niobate particles according to the embodiment, it is preferable to further use a molybdenum compound. By using the molybdenum compound, crystal growth of the niobate particles can be further promoted, and the niobate particles can be produced with high efficiency.
[0076] An example of a method for producing such niobate particles includes a method comprising calcining a niobium compound, or a niobium compound and a tantalum compound, in the presence of a molybdenum compound and a potassium compound and / or a sodium compound.
[0077] A preferred method for producing niobate particles can include a step of mixing a niobium compound, or a niobium compound and a tantalum compound, with a molybdenum compound, and a potassium compound and / or a sodium compound to form a mixture (mixing step), and a step of firing the mixture (firing step).
[0078] Here, at least a part of the molybdenum compound and the potassium compound may be replaced with a compound containing molybdenum and potassium, such as potassium molybdate, and at least a part of the molybdenum compound and the sodium compound may be replaced with a compound containing molybdenum and sodium, such as sodium molybdate. Therefore, mixing of molybdenum with a compound containing potassium and / or sodium is also considered to be mixing of a molybdenum compound with a potassium compound and / or a sodium compound.
[0079] [Mixing process] The mixing step is a step of mixing a niobium compound, or a niobium compound and a tantalum compound, and optionally a molybdenum compound, and a potassium compound and / or a sodium compound to obtain a mixture.
[0080] When the niobate particles produced contain potassium sodium tantalate niobate, the method can include a step of mixing a niobium compound, a tantalum compound, and optionally a molybdenum compound, a potassium compound, and a sodium compound to form a mixture (mixing step).
[0081] When the niobate particles produced contain potassium sodium niobate, the method may include a step of mixing a niobium compound, and optionally a molybdenum compound, a potassium compound, and a sodium compound to form a mixture (mixing step).
[0082] When the niobate particles produced contain potassium niobate, the method may include a step of mixing a niobium compound, and optionally a molybdenum compound and a potassium compound to form a mixture (mixing step).
[0083] When the niobate particles produced contain sodium niobate, the method may include a step of mixing a niobium compound, and optionally a molybdenum compound and a sodium compound to form a mixture (mixing step).
[0084] The contents of the mixture will be described below.
[0085] (Niobium compounds) The niobium compound is not limited as long as it is a compound that can be converted into a niobate by firing together with a raw material compound, and examples thereof include niobium oxide, niobium hydroxide, niobium sulfide, niobium nitride, niobium fluoride, niobium chloride, niobium bromide, niobium iodide and other niobium halides, niobium alkoxides, and the like. Niobium hydroxide and niobium oxide are preferred, and niobium oxide is more preferred. Examples of niobium oxide include niobium pentoxide (Nb2O5), niobium dioxide (NbO2), and niobium monoxide (NbO). In addition to the niobium oxides having the above oxidation numbers, any niobium oxide having a different valence can be used. The physical form, such as the shape, particle size, and specific surface area, of the niobium compound as the precursor is not particularly limited.
[0086] The shape after firing hardly reflects the shape of the raw material niobium compound, so any shape, such as a sphere, an amorphous shape, an aspected structure (wire, fiber, ribbon, tube, etc.), or a sheet, can be suitably used.
[0087] (Tantalum compounds) The tantalum compound is not limited as long as it is a compound that can be fired together with a raw material compound to become a tantalate, and examples thereof include tantalum oxide, tantalum hydroxide, tantalum sulfide, tantalum nitride, tantalum fluoride, tantalum chloride, tantalum bromide, tantalum iodide and other tantalum halides, and tantalum alkoxides. Tantalum hydroxide and tantalum oxide are preferred, and tantalum oxide is more preferred. Examples of tantalum oxide include tantalum pentoxide (Ta2O5), tantalum dioxide (TaO2), and tantalum monoxide (TaO). In addition to the tantalum oxides with the above oxidation numbers, any tantalum oxide with a different valence can be used. The physical form, such as the shape, particle size, and specific surface area, of the tantalum compound as the precursor is not particularly limited.
[0088] The shape of the sintered product does not substantially reflect the shape of the raw tantalum compound, and therefore any shape, such as a sphere, an amorphous structure with an aspect (wire, fiber, ribbon, tube, etc.), or a sheet, can be suitably used.
[0089] (Molybdenum Compounds) The molybdenum compound includes molybdenum oxide, molybdic acid, molybdenum sulfide, molybdate compounds, etc., and molybdenum oxide or molybdate compounds are preferred.
[0090] The molybdenum oxide includes molybdenum dioxide (MoO2), molybdenum trioxide (MoO3), etc., with molybdenum trioxide being preferred.
[0091] The molybdate compound is preferably an alkali metal salt of a molybdenum oxoanion, more preferably lithium molybdate, potassium molybdate or sodium molybdate, and even more preferably potassium molybdate or sodium molybdate.
[0092] In the method for producing niobate particles of this embodiment, the molybdenum compound may be a hydrate.
[0093] The molybdenum compound is preferably at least one compound selected from the group consisting of molybdenum trioxide, lithium molybdate, potassium molybdate, and sodium molybdate, and more preferably at least one compound selected from the group consisting of molybdenum trioxide, potassium molybdate, and sodium molybdate.
[0094] A compound containing molybdenum and potassium suitable as a fluxing agent can be produced, for example, in the firing process using a molybdenum compound and a potassium compound, which are cheaper and more readily available, as raw materials. Here, the use of a molybdenum compound and a potassium compound as fluxing agents and the use of a compound containing molybdenum and potassium as fluxing agents are both considered to be the use of a molybdenum compound and a potassium compound as fluxing agents, i.e., in the presence of a molybdenum compound and a potassium compound.
[0095] A compound containing molybdenum and sodium suitable as a fluxing agent can be produced, for example, in the firing process using a molybdenum compound and a sodium compound, which are cheaper and more readily available, as raw materials. Here, the use of a molybdenum compound and a sodium compound as fluxing agents and the use of a compound containing molybdenum and sodium as fluxing agents are both considered to be the use of a molybdenum compound and a sodium compound as fluxing agents, i.e., in the presence of a molybdenum compound and a sodium compound.
[0096] The above-mentioned molybdenum compounds may be used alone or in combination of two or more kinds.
[0097] In addition, potassium molybdate (K2Mo n O 3n+1 , n=1 to 3) contains potassium and can therefore also function as a potassium compound, which will be described later.
[0098] In addition, sodium molybdate (Na2Mo n O 3n+1 , n=1 to 3) contains sodium and can therefore function as a sodium compound, which will be described later.
[0099] (Potassium compounds) The potassium compound is not particularly limited, but includes potassium chloride, potassium chlorite, potassium chlorate, potassium sulfate, potassium hydrogen sulfate, potassium sulfite, potassium hydrogen sulfite, potassium nitrate, potassium carbonate, potassium hydrogen carbonate, potassium acetate, potassium oxide, potassium bromide, potassium bromate, potassium hydroxide, potassium silicate, potassium phosphate, potassium hydrogen phosphate, potassium sulfide, potassium hydrogen sulfide, potassium molybdate, potassium tungstate, etc. In this case, the potassium compound includes isomers, as in the case of molybdenum compounds. Among these, it is preferable to use potassium carbonate, potassium hydrogen carbonate, potassium oxide, potassium hydroxide, potassium chloride, potassium sulfate, and potassium molybdate, and it is more preferable to use potassium carbonate, potassium hydrogen carbonate, potassium chloride, potassium sulfate, and potassium molybdate, and it is more preferable to use potassium carbonate and / or potassium molybdate.
[0100] The potassium compounds described above may be used alone or in combination of two or more kinds.
[0101] As described above, potassium molybdate contains molybdenum and can therefore function as the molybdenum compound described above.
[0102] (Sodium compounds) The sodium compound is not particularly limited, and examples thereof include sodium carbonate, sodium molybdate, sodium oxide, sodium sulfate, sodium hydroxide, sodium nitrate, sodium chloride, metallic sodium, etc. Among these, from the viewpoint of industrially easy availability and ease of handling, it is preferable to use sodium carbonate, sodium molybdate, sodium oxide, and sodium sulfate, and it is more preferable to use sodium carbonate and / or sodium molybdate.
[0103] The above-mentioned sodium compounds may be used alone or in combination of two or more kinds.
[0104] As described above, sodium molybdate contains molybdenum and can therefore function as the molybdenum compound described above.
[0105] In this way, there may be cases where the molybdenum compound is classified as a molybdenum compound in a redundant manner. As an example, the molybdenum compound is at least one compound selected from the group consisting of molybdenum trioxide, potassium molybdate, and sodium molybdate, It is preferable that the sodium compound is sodium carbonate or sodium molybdate, and the potassium compound is potassium carbonate or potassium molybdate.
[0106] A preferred example of the method for producing potassium sodium niobate particles includes a method for firing a niobium compound in the presence of a molybdenum compound, a potassium compound and a sodium compound.
[0107] A preferred example of the method for producing sodium niobate particles includes a method for firing a niobium compound in the presence of a molybdenum compound and a sodium compound.
[0108] A preferred example of the method for producing potassium niobate particles includes a method for firing a niobium compound in the presence of a molybdenum compound and a potassium compound.
[0109] A preferred example of the method for producing potassium sodium tantalate niobate particles includes a method for firing a niobium compound and a tantalum compound in the presence of a molybdenum compound, a potassium compound and a sodium compound.
[0110] A preferred example of the method for producing potassium sodium tantalate niobate particles includes a method for firing a niobium compound and a tantalum compound in the presence of a potassium compound and a sodium compound.
[0111] In the method for producing niobate particles of this embodiment, the potassium compound, the sodium compound, and the molybdenum compound are used as fluxing agents. When a potassium compound and / or a sodium compound is used as a fluxing agent, it is presumed that an oxide (NaO or KO) is formed from a part of the potassium compound and / or sodium compound by such firing, and this functions as a flux to promote the crystal growth of niobate.
[0112] Furthermore, it is presumed that when a niobium compound is fired in the presence of potassium carbonate and / or sodium carbonate, some of the potassium carbonate and / or sodium carbonate forms oxides (Na2O or KO) and / or CO2, and these oxides and / or CO2 function as fluxes to promote crystal growth of niobate particles. The firing reaction forms oxides (Na2O and K2O) and / or CO2 that act as fluxes, and niobate particles (K x Na (1-x) Nb y Ta (1-y) O3) is thought to be formed. The oxides (Na2O and K2O) and / or CO2 function as fluxes, and niobate particles (K x Na (1-x) Nb y Ta (1-y) O3) is thought to be promoted.
[0113] When a molybdenum compound is used as a fluxing agent, the niobium compound or the niobium compound and the tantalum compound, the molybdenum compound, and the sodium compound or potassium compound (including the case of a compound containing molybdenum and sodium, or a compound containing molybdenum and potassium) react at high temperature to produce a molybdate compound (e.g., K a Mo b O c OrNa a Mo b O c , Ka Na a’ Mo b O c ) with the formation of niobate particles (K x Na (1-x) Nb y Ta (1-y) O3) is considered to be formed. When the niobate particles are formed (crystal growth), some of the molybdenum compounds are considered to be incorporated into the niobate particles. More specifically, regarding the mechanism of formation of the molybdenum compounds contained in the niobate particles, it is considered that the molybdenum compounds, for example, molybdenum oxides, are formed in the process of crystal growth of the niobate particles through the formation and decomposition of Mo-O-Nb or Mo-O-Ta in the system during firing, or through the molybdate compounds that are fluxing agents. Furthermore, in consideration of the above mechanism, it is also considered that the molybdenum oxides are present on the surface of the niobate particles through the bonds of Mo-O-Nb or Mo-O-Ta. The inclusion of molybdenum compounds (for example, molybdenum oxides) in the niobate particles leads to improvement in the physical properties of the niobate particles, and for example, the catalytic performance of the niobate particles can be improved.
[0114] The molybdate compound as the flux does not vaporize even in the firing temperature range and can be easily recovered by washing after firing, so that the amount of molybdenum compound released outside the firing furnace is reduced, and production costs can be significantly reduced.
[0115] In the method for producing niobate particles of this embodiment, the total amount of the raw molybdenum compound, potassium compound, and sodium compound (hereinafter also referred to as fluxing agent), which are considered to function as a fluxing agent, and the amount of the niobium compound and tantalum compound used are not particularly limited, but preferably, 10 parts by mass or more of the fluxing agent can be mixed with 100 parts by mass of the total amount of the raw niobium compound and tantalum compound used to prepare a mixture, and the mixture can be fired. More preferably, 20 to 5000 parts by mass of the fluxing agent can be mixed with 100 parts by mass of the total amount of the niobium compound and tantalum compound used to prepare a mixture, and the mixture can be fired. Even more preferably, 100 to 1000 parts by mass of the fluxing agent can be mixed with 100 parts by mass of the total amount of the niobium compound and tantalum compound used to prepare a mixture, and the mixture can be fired.
[0116] From the viewpoint of efficient crystal growth, it is preferable that the amount of fluxing agent used relative to the raw material niobium compound is equal to or greater than the lower limit. By increasing the amount of fluxing agent used relative to the raw material niobium compound, it is easy to control the crystallite size of the niobate particles produced, and niobate particles with improved crystallite size can be easily obtained. On the other hand, from the viewpoint of reducing the amount of fluxing agent used and improving production efficiency, it is preferable that the amount is equal to or less than the upper limit. If the amount of fluxing agent is large, large single crystals may be produced, which may reduce productivity, so the amount of flux can be appropriately selected so that the particle size of the niobate particles produced is the desired size.
[0117] From a similar viewpoint, in the method for producing niobate particles of the embodiment, the molar ratio (K+Na) / (Nb+Ta) of potassium atoms and sodium atoms to niobium atoms and tantalum atoms in the mixture is preferably 1.1 or more, more preferably 1.5 to 10, even more preferably 2.0 to 5, and particularly preferably 2.0 to 2.7. When the molar ratio (K+Na) / (Nb+Ta) is within the above range, niobate particles having an improved crystallite size can be easily obtained. The ratio of (K + Na) / (Nb + Ta) in the niobate particles (K x Na (1-x) Nb y Ta (1-y) O3) having a perovskite structure to be produced is usually around (K + Na) / (Nb + Ta) = 1 (a value within the range having a perovskite structure), and the excess (K + Na) in the mixture is considered to contribute to good crystal growth of the niobate as a so-called self-flux.
[0118] In the method for producing niobate particles according to the embodiment, the molar ratio of potassium atoms and / or sodium atoms to molybdenum atoms in the mixture is preferably (K + Na) / Mo = 1 to 4, more preferably 1.5 to 4. In particular, when (K + Na) / Mo = 2 to 4, K x Na (1-x) Nb y O z of a single composition can be easily formed.
[0119] In the method for producing niobate particles according to the embodiment, the ratio of K / Na of the produced niobate particles can be changed according to the blending ratio of K / Na of the raw materials. The molar ratio of potassium atoms and / or sodium atoms to molybdenum atoms in the mixture may be appropriately adjusted according to the desired values of X and 1 - X of K x Na (1-x) Nb y Ta (1-y) O3. When 0 < X < 1 for the X, the molar ratio of potassium atoms to sodium atoms in the mixture may be, for example, K / Na = 0.01 to 10, and may be 0.1 to 5.
[0120] By using various compounds within the above range, the amount of the molybdenum compound contained in the obtained niobate particles becomes more appropriate, and niobate particles with a controlled crystal shape can be easily obtained.
[0121] [Firing step] The firing step is a step of firing the mixture. The niobate particles according to the embodiment are obtained by firing the mixture. As described above, this manufacturing method is called a flux method.
[0122] The flux method is classified as a solution method. More specifically, the flux method is a crystal growth method that utilizes the fact that the crystal-flux two-component phase diagram shows a eutectic type. The mechanism of the flux method is presumed to be as follows. That is, when a mixture of a solute and flux is heated, the solute and flux become liquid phase. At this time, since the flux is a flux, in other words, since the solute-flux two-component phase diagram shows a eutectic type, the solute melts at a temperature lower than its melting point and forms a liquid phase. If the flux is evaporated in this state, the concentration of the flux decreases, in other words, the effect of the flux in lowering the melting point of the solute is reduced, and the evaporation of the flux becomes the driving force to cause crystal growth of the solute (flux evaporation method). Note that the solute and flux can also cause crystal growth of the solute by cooling the liquid phase (slow cooling method).
[0123] The flux method has the advantages of being able to grow crystals at temperatures much lower than the melting point, being able to precisely control the crystal structure, and being able to form idiomorphic crystals.
[0124] In the production of niobate particles by the flux method, when a niobium compound is fired in the presence of a potassium compound and / or a sodium compound, it is presumed that an oxide (NaO or KO) is formed from a portion of the potassium compound and / or sodium compound, and this functions as a flux to promote the crystal growth of the niobate particles. Furthermore, it is presumed that when a niobium compound is fired in the presence of potassium carbonate and / or sodium carbonate, some of the potassium carbonate and / or sodium carbonate forms oxides (Na2O or KO) and / or CO2, and these oxides and / or CO2 function as fluxes to promote crystal growth of niobate particles.
[0125] The mechanism by which niobate particles are produced when a molybdenum compound is used as a flux is not entirely clear, but it is presumed to be due to the following mechanism, for example. That is, when a niobium compound is fired in the presence of a molybdenum compound, some of the niobium compound forms niobium molybdate, and the molybdenum compound produces molybdate (e.g., K a Mo b O c OrNa a Mo b O c , K a Na a’ Mo b O c ) is formed. At this time, as can be understood from the above explanation, the flux function of the molybdate allows niobate crystals to grow at a temperature lower than the melting point of the niobate. In addition, for example, the partially formed niobium molybdate decomposes, promoting the crystal growth of the niobate particles. That is, the molybdenum compound (molybdate) functions as a flux, and niobate particles are produced via an intermediate called niobium molybdate.
[0126] The above mechanism is the same even when a niobium compound and a tantalum compound are fired in place of the niobium compound.
[0127] The method of calcination is not particularly limited, and can be a known, commonly used method. When a molybdenum compound is used, if the calcination temperature exceeds 500° C., some of the niobium compound or tantalum compound reacts with the molybdenum compound to form niobium molybdate, etc., and the molybdenum compound produces molybdate (K a Mo b O c OrNa a Mo b O c , K a Na a’ Mo b O c) is thought to be formed. Furthermore, when the firing temperature reaches 800°C or higher, it is thought that the partially formed niobium molybdate etc. decomposes, and niobate particles are formed due to the flux function of the molybdate. In addition, it is thought that in the niobate particles, molybdenum compounds are taken into the niobate particles during the process of decomposition of niobium molybdate and particle crystal growth.
[0128] In addition, the state of the niobium compound, tantalum compound, molybdenum compound, sodium compound, potassium compound, etc. that can be used in firing is not particularly limited, and it is sufficient that the raw material compounds such as the molybdenum compound, the niobium compound, the tantalum compound, the sodium compound, the potassium compound, etc. are present in the same space so that they can interact with each other. Specifically, simple mixing in which powders of the raw material compounds are mixed together, mechanical mixing using a grinder or the like, mixing using a mortar or the like, and mixing in a dry state or a wet state may be used.
[0129] The firing temperature condition is not particularly limited, and is appropriately determined in consideration of the particle size of the target niobate particles, the formation of the molybdenum compound in the niobate particles, the shape of the niobate particles, etc. The firing temperature may be 700°C or higher, which is close to the temperature at which the molybdate can function as a flux, or 750°C or higher, 800°C or higher, 850°C or higher, or 900°C or higher. From the viewpoint of efficiently producing niobate particles with an improved crystallite size, the firing temperature is preferably 800° C. or higher, more preferably 900° C. or higher, and even more preferably 1000° C. or higher.
[0130] Generally, to control the shape of niobate obtained after firing, it is necessary to perform high-temperature firing at over 1500°C, which is close to the melting point of niobium oxide. However, there are significant challenges to be overcome in terms of the burden on the firing furnace and fuel costs in order to utilize this industrially.
[0131] According to one embodiment of the present invention, even under conditions where the maximum sintering temperature for sintering a niobium compound is 1500° C. or lower, niobate particles can be formed efficiently at low cost. Furthermore, according to the method for producing niobate particles of the embodiment, idiomorphous niobate particles can be formed regardless of the shape of the precursor even at a firing temperature of 1300° C. or less, which is much lower than the melting point of niobium oxide. From the viewpoint of efficiently producing niobate particles, the firing temperature is preferably 1200° C. or less, and more preferably 1100° C. or less.
[0132] The numerical range of the firing temperature for firing the niobium compound in the firing step may be, for example, 700 to 1300°C, 750 to 1300°C, 800 to 1200°C, 850 to 1200°C, 900 to 1100°C, or 1000 to 1100°C.
[0133] From the viewpoint of production efficiency, the temperature rise rate may be 20 to 600° C. / h, 40 to 500° C. / h, or 80 to 400° C. / h.
[0134] Regarding the firing time, it is preferable that the time required to raise the temperature to a predetermined firing temperature is within the range of 15 minutes to 10 hours, and that the time required to hold the firing temperature is within the range of 5 minutes to 30 hours. In order to efficiently form niobate particles, the firing temperature is preferably held for 2 hours or more, and more preferably for 2 to 15 hours. Niobate particles having an improved crystallite size can be easily obtained by selecting conditions of a firing temperature of 700 to 1100° C. and a firing temperature holding time of 2 to 15 hours.
[0135] The firing atmosphere is not particularly limited as long as the effects of the present invention can be obtained. For example, an oxygen-containing atmosphere such as air or oxygen, or an inert atmosphere such as nitrogen, argon, or carbon dioxide is preferable, and an air atmosphere is more preferable in terms of cost.
[0136] The calcination apparatus is not necessarily limited, and a so-called calcination furnace can be used. The calcination furnace is preferably made of a material that does not react with the sublimated molybdenum oxide, and it is preferable to use a highly airtight calcination furnace so as to efficiently utilize the molybdenum oxide.
[0137] [Cooling process] The method for producing niobate particles may include a cooling step, which is a step of cooling the niobate particles whose crystals have been grown in the firing step.
[0138] The cooling rate is not particularly limited, but is preferably 1 to 1000°C / hour, more preferably 5 to 500°C / hour, and even more preferably 50 to 100°C / hour. A cooling rate of 1°C / hour or more is preferable because the manufacturing time can be shortened. On the other hand, a cooling rate of 1000°C / hour or less is preferable because the firing container is less likely to crack due to heat shock and can be used for a long time.
[0139] The cooling method is not particularly limited, and may be natural cooling or a cooling device may be used.
[0140] [Post-processing process] The manufacturing method of this embodiment may include a post-treatment step. The post-treatment step may be a step of separating the niobate particles and the flux agent contained in the fired product, and may be performed by removing the fired product from the firing vessel. The post-treatment step may be performed after the above-mentioned firing step. In addition, the post-treatment step may be repeated two or more times as necessary.
[0141] Methods for removing the fluxing agent include cleaning, high temperature treatment, etc. These may be used in combination.
[0142] The cleaning method is not particularly limited, but when the flux is water-soluble like the potassium compounds, sodium compounds, and molybdate compounds, washing with water is an example.
[0143] As a method of high temperature treatment, a method of raising the temperature to the sublimation point or boiling point of the flux or higher can be mentioned.
[0144] [Crushing process] In the fired product obtained through the firing step, the niobate particles may aggregate and may not satisfy the suitable particle size range for the intended application. Therefore, the niobate particles may be pulverized as necessary to satisfy the suitable particle size range. The method for pulverizing the fired product is not particularly limited, and any conventionally known pulverizing method such as a ball mill, a jaw crusher, a jet mill, a disk mill, a spectromill, a grinder, or a mixer mill can be used.
[0145] [Classification process] The fired product containing niobate particles obtained by the firing step may be appropriately classified to adjust the range of particle size. "Classification" refers to an operation of grouping particles according to their size. The classification may be either wet or dry, but from the viewpoint of productivity, dry classification is preferred. Dry classification includes classification by sieving, as well as wind classification, which classifies based on the difference between centrifugal force and fluid drag, but from the viewpoint of classification accuracy, wind classification is preferred, and can be performed using a classifier such as an air classifier utilizing the Coanda effect, a swirling air classifier, a forced vortex centrifugal classifier, or a semi-free vortex centrifugal classifier. The above-mentioned pulverization step and classification step can be carried out at any stage required. Depending on whether or not the pulverization or classification is carried out and the selection of the conditions therefor, for example, the average particle size of the obtained niobate particles can be adjusted.
[0146] The niobate particles of the embodiment, or the niobate particles obtained by the manufacturing method of the embodiment, are preferably those which are less aggregated or are not aggregated, from the viewpoints of easily exerting their inherent properties, being more easily handled, and being more dispersible when dispersed in a dispersion medium.
[0147] According to the method for producing niobate particles of the above embodiment, niobate particles with little or no agglomeration can be easily produced, and therefore, even without carrying out the above-mentioned crushing step or classification step, it has an excellent advantage that niobate particles having the desired excellent properties can be produced with high productivity.
[0148] ≪Resin composition≫ The niobate particles of the embodiment can be blended with a resin to provide a resin composition. As an embodiment, a resin composition containing the niobate particles of the embodiment and a resin is provided. The resin is not particularly limited, and may be a polymer, an oligomer, or a monomer, a thermosetting resin, a thermoplastic resin, or an active energy ray-curable resin.
[0149] (thermosetting resin) The thermosetting resin is a resin that has the property of being changed to be substantially insoluble and infusible when cured by means of heat, radiation, a catalyst, etc. For example, it may be a known and commonly used resin used in molding materials, etc. Specific examples of the resin include novolac-type phenolic resins such as phenol novolac resin and cresol novolac resin; phenolic resins such as unmodified resol phenolic resin and resol-type phenolic resin such as oil-modified resol phenolic resin modified with tung oil, linseed oil, walnut oil, etc.; bisphenol-type epoxy resins such as bisphenol A epoxy resin and bisphenol F epoxy resin; novolac-type epoxy resins such as aliphatic chain-modified bisphenol-type epoxy resin, novolac epoxy resin, cresol novolac epoxy resin; epoxy resins such as biphenyl-type epoxy resin and polyalkylene glycol-type epoxy resin; resins having a triazine ring such as urea resin and melamine resin; vinyl resins such as (meth)acrylic resin and vinyl ester resin; unsaturated polyester resin, bismaleimide resin, polyurethane resin, diallyl phthalate resin, silicone resin, resin having a benzoxazine ring, cyanate ester resin, etc., and may be a polymer, oligomer, or monomer.
[0150] The above-mentioned thermosetting resin may be used together with a curing agent. The curing agent used in this case may be used in a known and commonly used combination with the thermosetting resin. For example, when the thermosetting resin is an epoxy resin, any compound commonly used as a curing agent may be used, such as an amine-based compound, an amide-based compound, an acid anhydride-based compound, or a phenol-based compound. Specifically, examples of the amine-based compound include diaminodiphenylmethane, diethylenetriamine, triethylenetetramine, diaminodiphenylsulfone, isophoronediamine, imidazole, BF3-amine complex, and guanidine derivatives. Examples of the amide-based compounds include dicyandiamide, polyamide resins synthesized from a dimer of linolenic acid and ethylenediamine, etc. Examples of the acid anhydride-based compounds include phthalic anhydride, trimellitic anhydride, pyromellitic anhydride, maleic anhydride, tetrahydrophthalic anhydride, methyltetrahydrophthalic anhydride, methylnadic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, etc. Examples of the phenol-based compounds include phenol novolac resin, cresol novolac resin, aromatic hydrocarbon formaldehyde resin-modified phenol resin, dicyclopentadiene phenol addition type resin, phenol aralkyl resin (Zylok resin), polyhydric phenol novolac resins synthesized from polyhydric hydroxy compounds and formaldehyde, such as resorcinol novolac resin, naphthol aralkyl resin, trimethylol methane resin, tetraphenylol ethane resin, naphthol novolac resin, naphthol-phenol co-condensed novolac resin, naphthol-c Examples of the polyhydric phenol compounds include resol co-condensed novolac resin, biphenyl modified phenol resin (a polyhydric phenol compound in which a phenol nucleus is linked by a bismethylene group), biphenyl modified naphthol resin (a polyhydric naphthol compound in which a phenol nucleus is linked by a bismethylene group), aminotriazine modified phenol resin (a polyhydric phenol compound in which a phenol nucleus is linked by melamine, benzoguanamine, etc.), and alkoxy group-containing aromatic ring modified novolac resin (a polyhydric phenol compound in which a phenol nucleus and an alkoxy group-containing aromatic ring are linked by formaldehyde). These curing agents may be used alone or in combination of two or more kinds.
[0151] The blending amounts of the thermosetting resin and the curing agent in the resin composition of the embodiment are not particularly limited. For example, when the curable resin is an epoxy resin, it is preferable to use an amount such that the active groups in the curing agent are 0.7 to 1.5 equivalents per total equivalent of the epoxy groups in the epoxy resin, since this will result in good properties of the cured product.
[0152] If necessary, a curing accelerator can be used in combination with the thermosetting resin in the resin composition of the embodiment. For example, when the curing resin is an epoxy resin, various curing accelerators can be used, such as phosphorus compounds, tertiary amines, imidazoles, organic acid metal salts, Lewis acids, and amine complex salts.
[0153] If necessary, a curing catalyst can be used in combination with the thermosetting resin at appropriate times, and examples of such a catalyst include well-known and commonly used thermal polymerization initiators and active energy ray polymerization initiators.
[0154] (thermoplastic resin) Examples of thermoplastic resins that may be used in the resin composition of the embodiment include known and commonly used resins used in molding materials, etc. Specific examples include polyethylene resins, polypropylene resins, polymethyl methacrylate resins, polyvinyl acetate resins, ethylene-propylene copolymers, ethylene-vinyl acetate copolymers, polyvinyl chloride resins, polystyrene resins, polyacrylonitrile resins, polyamide resins, polycarbonate resins, polyacetal resins, polyethylene terephthalate resins, polyphenylene oxide resins, polyphenylene sulfide resins, polysulfone resins, polyethersulfone resins, polyetheretherketone resins, polyarylsulfone resins, thermoplastic polyimide resins, thermoplastic urethane resins, polyaminobismaleimide resins, polyamideimide resins, polyetherimide resins, bismaleimide triazine resins, polymethylpentene resins, fluorinated resins, liquid crystal polymers, olefin-vinyl alcohol copolymers, ionomer resins, polyarylate resins, acrylonitrile-ethylene-styrene copolymers, acrylonitrile-butadiene-styrene copolymers, acrylonitrile-styrene copolymers, etc. At least one thermoplastic resin can be selected and used, but two or more thermoplastic resins can also be used in combination depending on the purpose.
[0155] When the resin is used for a piezoelectric body, it is preferable that the resin exhibits a high dielectric constant, and the resin is preferably a polymer having an electron-withdrawing group, and is preferably a fluorine-containing polymer such as polyvinylidene fluoride (PVDF), vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, or a polymer having a cyano group or a cyanoethyl group such as cyanoethylated polyvinyl alcohol, vinylidene cyanide-vinyl acetate copolymer, cyanoethyl cellulose, cyanoethyl hydroxysaccharose, cyanoethyl hydroxycellulose, cyanoethyl hydroxypullulan, cyanoethyl methacrylate, cyanoethyl acrylate, cyanoethyl hydroxyethyl cellulose, cyanoethyl amylose, cyanoethyl hydroxypropyl cellulose, cyanoethyl dihydroxypropyl cellulose, cyanoethyl hydroxypropyl amylose, cyanoethyl polyacrylamide, cyanoethyl polyacrylate, cyanoethyl pullulan, cyanoethyl polyhydroxymethylene, cyanoethyl glycidol pullulan, cyanoethyl saccharose, and cyanoethyl sorbitol.
[0156] The resin composition of the embodiment may contain other compounds as necessary, and may contain external lubricants, internal lubricants, antioxidants, flame retardants, light stabilizers, ultraviolet absorbers, silane, titanate, or aluminate coupling agents, reinforcing materials such as glass fiber or carbon fiber, fillers, various colorants, etc., within the scope of the effects of the invention. In addition, it is also possible to use stress reducing agents (stress relaxation agents) such as silicone oil, liquid rubber, rubber powder, butadiene copolymer rubber such as methyl acrylate-butadiene-styrene copolymer or methyl methacrylate-butadiene-styrene copolymer, and silicone compounds.
[0157] The resin composition of the embodiment is obtained by mixing the niobate particles of the embodiment, a resin, and, if necessary, other ingredients. There is no particular limitation on the mixing method, and the ingredients are mixed by a known and commonly used method.
[0158] In the case where the resin is a thermosetting resin, a general method is to thoroughly mix the thermosetting resin, the niobate particles of the embodiment, and other components as necessary with a mixer or the like, and then knead them with a three-roll mill or the like to obtain a fluid liquid composition, or to thoroughly mix a predetermined amount of the thermosetting resin, the niobate particles of the embodiment, and other components as necessary with a mixer or the like, and then melt-knead them with a mixing roll, extruder, or the like, and then cool them to obtain a solid composition. When a curing agent, catalyst, or the like is added, it is preferable that the curable resin and the compounded material are thoroughly and uniformly mixed, and it is more preferable that the niobate particles of the embodiment are also uniformly dispersed and mixed.
[0159] A typical method when the resin is a thermoplastic resin is to mix the thermoplastic resin, the niobate particles of the embodiment, and other components as necessary in advance using various mixers such as a tumbler or a Henschel mixer, and then melt-knead using a mixer such as a Banbury mixer, a roll, a Brabender, a single-screw kneading extruder, a twin-screw kneading extruder, a kneader, a mixing roll, etc. The temperature for melt-kneading is not particularly limited, but may be in the range of 240 to 320°C.
[0160] When preparing the resin composition of the embodiment, the mixing ratio of the niobate particles of the embodiment to the non-volatile content of the resin is not particularly limited, but may be, for example, in the range of 0.1 to 1800 parts of the niobate particles, or in the range of 10 to 900 parts, per 100 parts by mass of the non-volatile content of the resin.
[0161] The content ratio of the niobate particles relative to the total mass (100 mass%) of the resin composition of the embodiment may be 30 mass% or more, may be 50 to 90 mass%, or may be 60 to 85 mass%.
[0162] <Molded body> A molded article can be obtained by molding the resin composition of the embodiment. As one embodiment, a molded article is provided by molding the resin composition of the embodiment. The resin molded article can be obtained by a known and commonly used method.
[0163] For example, when the resin contained in the resin composition is a thermosetting resin, the curing method may conform to that of a thermosetting resin composition such as a general epoxy resin composition. For example, a resin composition in which the resin is an epoxy resin may be cured by heat, and the heating temperature conditions may be appropriately selected depending on the type of curing agent to be combined and the application, and the resin may be heated in a temperature range of about room temperature to 250°C. In the case of an active energy ray curable resin, the resin may be cured and molded by irradiating it with active energy rays such as ultraviolet rays or infrared rays.
[0164] In addition, even when the resin of the embodiment is a thermoplastic resin, it can be molded into a molded product by a known and commonly used molding method. For example, there are injection molding, ultra-high speed injection molding, injection compression molding, two-color molding, gas-assisted and other hollow molding methods, molding methods using a heat-insulating mold, molding methods using a rapidly heated mold, foam molding (including supercritical fluid), insert molding, IMC (in-mold coating molding) molding, extrusion molding, sheet molding, rotational molding, lamination molding, press molding, and the like. In addition, a molding method using a hot runner system can also be used. There are no limitations on the shape, pattern, color, dimensions, etc. of the molded product, and they may be set arbitrarily according to the application of the molded product.
[0165] When the molded article of the resin composition is in the form of a sheet or layer, its thickness may be 10 to 100 μm, or 10 to 80 μm.
[0166] The resin composition of the embodiment and a molded product thereof can be provided and used as a piezoelectric body by appropriately carrying out a polarization treatment. EXAMPLES
[0167] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to the following examples.
[0168] <Analysis and Evaluation> The powders of each of the Examples and Comparative Examples were used as samples to carry out the following measurements.
[0169] [XRF (X-ray fluorescence) analysis] Using a Primus IV X-ray fluorescence analyzer (Rigaku Corporation), approximately 70 mg of the sample powder was placed on filter paper, covered with PP film, and subjected to XRF (X-ray fluorescence) analysis under the following conditions. EZ Scan Mode Measuring elements: F~U Measurement time: Standard Measurement diameter: 10mm Balance: None
[0170] The sample powder was subjected to XRF analysis to determine the niobium content in the sample powder, and the niobium content was calculated as the content (mass %) in terms of Nb2O5 relative to 100 mass % of the total mass of the sample powder. The sample powder was subjected to XRF analysis to determine the tantalum content in the sample powder, and the content was calculated as the content (mass %) in terms of Ta2O5 relative to 100 mass % of the total mass of the sample powder. The sample powder was subjected to XRF analysis to determine the molybdenum content in the sample powder, and the molybdenum content was calculated as the content (mass %) in terms of MoO3 relative to 100 mass % of the total mass of the sample powder. The sample powder was subjected to XRF analysis to determine the potassium content in the sample powder, and the content was calculated as the content (mass%) in terms of K2O relative to 100% by mass of the total mass of the sample powder. The sample powder was subjected to XRF analysis to determine the sodium content in the sample powder, and the content (mass%) in terms of Na2O relative to 100% by mass of the total mass of the sample powder.
[0171] [Crystal structure analysis: XRD (X-ray diffraction) method] The sample powder was filled into a measurement sample holder with a depth of 0.5 mm, which was then set in a wide-angle X-ray diffraction (XRD) device (Ultima IV, manufactured by Rigaku Corporation) and subjected to a Cu / Kα ray diffraction (Cu / Kα ray diffraction) at 40 k The measurements were performed under conditions of V / 40 mA, scan speed 2° / min, and scan range 10 to 70° or scan range 10 to 90°.
[0172] [Calculation of x from XRD shift] Ta-free K x Na (1-x) For NbO3, the XRD peak positions are based on the data reported previously (Bo-Ping Zhang et al. J. Am. Ceram. Soc., 89 [5] 1605-1609 (2006)). and the composition x was determined by interpolation.
[0173] [Particle size measurement] (For particles with cubic shapes) The sample powder was photographed with a scanning electron microscope (SEM). For the smallest unit particle (i.e., primary particle) observed in the two-dimensional image, if it was observed to have a cubic shape, the length of one side of the hexahedron determined from the particle image of the primary particle was measured as the particle size. The same procedure was carried out for 50 primary particles, and the average value for each was calculated.
[0174] [Crystallite size measurement] The measurement was performed using a SmartLab (Rigaku Corporation) as an X-ray diffraction device, a high intensity, high resolution crystal analyzer (CALSA) as a detector, and PDXL as an analysis software. The measurement method was the 2θ / θ method, and the average crystallite size was calculated using the Scherrer formula from the half-width of the peaks appearing at 2θ=23.0±1.0°, 2θ=32.0±1.2°, and 2θ=57.0±1.0°. The measurement conditions were a scan speed of 0.05° / min, a scan range of 20-70°, a step of 0.002°, and a standard width of the device of 0.028°(Si).
[0175] [Particle size distribution measurement] The particle size distribution of the sample powder was measured in a dry state using a laser diffraction type dry particle size distribution analyzer (HELOS (H3355) & RODOS, manufactured by Japan Laser Co., Ltd.) under the conditions of a dispersion pressure of 3 bar and a suction pressure of 90 mbar. The particle size at the point where the distribution curve of the volume cumulative percentage intersects with the horizontal axis of 50% was defined as D. 50 The particle diameter at the point where the volume cumulative % distribution curve intersects with the horizontal axis at 10% from the small particle side is D.10 The particle diameter at the point where the volume cumulative % distribution curve intersects with the horizontal axis at 90% from the small particle side is D. 90 was requested as follows.
[0176] [Specific surface area measurement] The specific surface area of the sample powder was measured using a specific surface area meter (Microtrack-Bel, BELSORP-mini), and the surface area per 1 g of sample measured from the amount of nitrogen gas adsorbed by the BET method was defined as the specific surface area (m 2 / g).
[0177] <1.K x Na (1-x) Nb y Ta (1-y) Production of O3 particles> [Example 1] A mixture was obtained by mixing 10.0 g of niobium oxide (reagent manufactured by Kanto Chemical Co., Ltd., Nb2O5), 6.8 g of molybdenum oxide (reagent manufactured by Kanto Chemical Co., Ltd., MoO3), 7.53 g of potassium carbonate (reagent manufactured by Kanto Chemical Co., Ltd., K2CO3), and 4.0 g of sodium carbonate (reagent manufactured by Kanto Chemical Co., Ltd., Na2CO3) in a mortar. The resulting mixture was placed in a crucible and fired in a ceramic electric furnace at 1100°C for 10 hours. After cooling, the crucible was removed from the ceramic electric furnace. The fired product was then ultrasonically washed five times with water, and then washed with water to remove the washing water by filtration, and then dried to remove the remaining flux agent, thereby obtaining 10.8 g of powder of Example 1.
[0178] The synthesis conditions are shown in Table 1.
[0179] [Table 1]
[0180] [Examples 2 to 13] Powders of Examples 2 to 13 were obtained in the same manner as in Example 1, except that the composition of the raw materials and the firing temperature in Example 1 were changed as shown in Table 1. As the raw material Ta2O5 in Table 1, tantalum oxide (reagent, Ta2O5, manufactured by Kanto Chemical Co., Ltd.) was used.
[0181] [Comparative Example 1] Commercially available potassium sodium niobate (manufactured by Nippon Chemical Industry Co., Ltd.) was used as the powder in Comparative Example 1.
[0182] <Result> SEM images of the powders of Examples 1 to 13 and Comparative Example 1 are shown in FIGS.
[0183] The results of each of the above evaluations are shown in Table 2. "-" indicates that the corresponding compound was not used. "ND" stands for "not detected."
[0184] [Table 2]
[0185] Table 2 shows the shape and size of particles in each of the examples and comparative examples as determined from SEM images. When particles of different shapes were observed to be mixed, the representative shape (the shape most commonly observed) was recorded. Cubic particle aggregates were also recorded as having a cubic shape. When no specific shape was observed, the material was judged to be amorphous.
[0186] The results of the XRD analysis are shown in Figures 15 to 19. In each of the samples of Examples 1 to 5, K x Na (1-x) Peaks at 2θ=23.0±1.0°, 2θ=32.0±1.2°, and 2θ=57.0±1.0° were observed, which were derived from the (100), (110), and (221) planes of the perovskite structure of NbO3.
[0187] In the sample of Example 6, peaks were observed at 2θ=23.0±1.0°, 2θ=32.0±1.2°, and 2θ=57.0±1.0°, respectively, originating from the (100) plane, (110) plane, and (221) plane of the perovskite structure of NaNbO3. In the sample of Example 7, peaks were observed at 2θ=23.0±1.0°, 2θ=32.0±1.2°, and 2θ=57.0±1.0°, respectively, originating from the (100) plane, (110) plane, and (221) plane of the perovskite structure of KNbO3.
[0188] In the samples of Examples 8 to 13, K x Na (1-x) Nb y Ta (1-y) Peaks at 2θ=23.0±1.0°, 2θ=32.0±1.2°, and 2θ=57.0±1.0° were observed, which were attributable to the (100), (110), and (221) planes of the perovskite structure of O3.
[0189] In the sample of Comparative Example 1, K x Na (1-x) Peaks at 2θ=23.0±1.0°, 2θ=32.0±1.2°, and 2θ=57.0±1.0° were observed, which were derived from the (100), (110), and (221) planes of the perovskite structure of NbO3.
[0190] From the results of the SEM observation and XRD analysis, it was found that the powders obtained in Examples 1 to 13 were cubic in shape and had a perovskite structure. x Na (1-x) Nb y Ta (1-y) It was confirmed to be an O3 particle.
[0191] Among the peaks shown above obtained by X-ray diffraction measurement, the ratio (R) of the peak intensity I(100) of the peak having a peak top at 2θ=23.0±1.0° to the peak intensity I(110) of the peak having a peak top at 2θ=32.0±1.2° was calculated. R=I(100) / I(110) The peak intensity was determined as the value at the peak top of the corresponding peak.
[0192] The values of R are shown in Table 2. As is clear from the results shown in Figures 15 to 19, the values of R were 1 or more in Examples 1 to 13, whereas the value of R in Comparative Example 1 was 0.9, which was lower than the values in the Examples. According to the results of SEM observation, it was confirmed that amorphous particles were mixed in the powder sample of Comparative Example 1. It is considered that in Comparative Example 1, the content of amorphous particles was high, which made it difficult for the particles to be oriented in the same direction during XRD measurement, and therefore more diffraction from the (110) plane was detected than from the (100) plane. From this, the powders obtained in Examples 1 to 13, in which the R value was 1 or more, had a uniform particle shape. x Na (1-x) It was shown to be of high quality, containing a large amount of NbO3 particles.
[0193] Moreover, the powder samples of Examples 1 to 13 were shown to contain niobium, tantalum, molybdenum, potassium, and sodium in the oxide-equivalent amounts shown in Table 2, which were determined by XRF analysis.
[0194] Each particle size (SEM observation, D 50 Focusing on the primary particle size and crystallite size, the particles of Examples 1 to 13 had larger primary particle size and crystallite size than the particles of Comparative Example. This is considered to be the result of the fact that the majority of the raw material compounds MoO3, Na2Co3, and K2CO3 (including their products and decomposition products) used in the manufacturing methods of each Example functioned as fluxing agents, allowing the crystal growth of the particles to proceed smoothly.
[0195] Furthermore, there was a tendency that the higher the firing temperature, the larger the particles obtained (Examples 1 to 5).
[0196] It was confirmed that each of the particles in Examples 1 to 13 and Comparative Example 1 had the BET specific surface area shown in Table 2.
[0197] From the results of Examples 1 to 13, it is possible to obtain high-quality K ferrite powder having a large average crystallite size and a perovskite structure by firing a niobium compound, or a niobium compound and a tantalum compound, in the presence of a potassium compound and / or a sodium compound. x Na (1-x) Nb y Ta (1-y) It was shown that O3 particles can be sintered.
[0198] In Examples 1 to 12 in which a molybdenum compound was used, K x Na (1-x) Nb y Ta (1-y) The yield calculated by the formula: actual yield of O3 particles / theoretical yield x 100 (mass%) was 80 mass% or more in all cases. However, in Example 13, which did not use a molybdenum compound, x Na (1-x) Nb y Ta (1-y) The yield of O3 particles was 28 mass %. From this, it can be seen that the use of molybdenum compounds x Na (1-x) Nb y Ta (1-y) It was demonstrated that O3 particles can be produced with high efficiency.
[0199] <2. Production of resin composition> 2.1.K x Na (1-x) Preparation of NbO3 particles [Example 14] Niobium oxide (Kanto Chemical Co., Ltd., Nb2O5) 40.3g, molybdenum oxide (Nihon Inorganic Chemical Industry Co., Ltd., MoO3) 27.21g, sodium carbonate (Kanto Chemical Co., Ltd., Na2CO3) x = 8.0g, and potassium carbonate (Kanto Chemical Co., Ltd., K2CO3) 46.1g-xg were mixed for 30 seconds in an absolute mill (Osaka Chemical Co., Ltd.) to obtain a mixture. The obtained mixture was divided and filled into four alumina crucibles, and fired at 900°C for 10 hours in a ceramic electric furnace. The obtained fired product was then placed in 250 mL of pure water, treated with an ultrasonic cleaner for 10 minutes, allowed to stand for 30 minutes, and decanted. This ultrasonic cleaning was repeated four times, and then dried to obtain the powder of Example 14.
[0200] The synthesis conditions are shown in Table 3.
[0201] [Table 3]
[0202] [Examples 15 to 17] Powders of Examples 15 to 17 were obtained in the same manner as in Example 14, except that the composition of the raw materials and the firing temperature in Example 14 were changed as shown in Table 3.
[0203] <Result> The results of each of the above evaluations are shown in Table 4. "-" indicates that the corresponding compound was not used. "ND" stands for "not detected."
[0204] [Table 4] From the results shown in Table 4, the powders obtained in Examples 14 to 17 were K having a perovskite structure. x Na (1-x) It was confirmed to be NbO3 particles.
[0205] 2.2. Production of resin composition A polymer solution was obtained by dissolving 30% by mass of cyanoethylated polyvinyl alcohol (Cyanoresin (registered trademark) CR-V, manufactured by Shin-Etsu Chemical Co., Ltd.) in 70% by mass of N,N-dimethylformamide. 7.33 g of this polymer solution and 13.5 g of the powder obtained in any of Examples 14 to 17 and Comparative Example 1 were placed in a vial and mixed for 2 minutes using a mixer (Thinky Corporation, Awatori Rentaro) to obtain the resin compositions of Examples 15 to 17 and Comparative Example 1.
[0206] <Evaluation of piezoelectric performance> To evaluate the piezoelectric performance, a simple speaker (Figure 20) was made using the following procedure.
[0207] A copper electrode having a thickness of 100 nm was deposited on a PET film 10 having a thickness of 50 μm using a deposition apparatus, and this was used as a lower electrode 20 . Using a Baker-type applicator (manufactured by Tester Sangyo, SA-201), the resin composition obtained above was applied onto the copper electrode so that the thickness after drying was 50 μm, forming a composite layer 30 (a molded body of the resin composition). Thereafter, the composite layer was dried for 10 minutes in a dryer at 80° C. During application, a part of the copper electrode was covered with masking tape so that a part of the copper electrode was exposed.
[0208] Using a corona discharge system (ELC-01N, manufactured by Element Ltd.), the copper electrode was earthed, the laminate obtained above was heated to 100°C, and a voltage of -7 kV was applied to the surface of the composite layer 30 to perform a polarization treatment.
[0209] The exposed portion of the lower electrode 20 and the periphery of the composite layer were masked with Kapton tape, and an Al electrode was vapor-deposited in an area slightly smaller than the area of the composite layer 30 to form an upper electrode 40.
[0210] The resulting laminate had PET film 10 (50 μm) / lower electrode 20 (Cu, 100 nm) / composite layer 30 (50 μm) / upper electrode 40 (Al, 100 nm) laminated in this order. Conductive tapes 61, 62 (copper foil, CU-35C, manufactured by 3M) were then attached to the lower electrode 20 and upper electrode 40, and the laminate was then sandwiched between O-rings 51, 52 to warp the composite layer.
[0211] A voltage of 1 kHz and 20 Vpp was applied through conductive tapes 61 and 62 clamped with alligator clips, and the sound pressure (a relative value with Comparative Example 1 being set at 1) was obtained by measuring with a microphone (Accor Corporation, 4152N) at a location 2 cm away from the composite layer.
[0212] The results are shown in Table 5. The molar ratio defined as K / (K+Na) in Table 5 is the content (mass%) calculated in terms of K2O and Na2O calculated by XRF analysis shown in Table 4. ) was calculated.
[0213] [Table 5]
[0214] The loudspeakers including the composite layers containing the powders of Examples 14 to 17 had much higher sound pressure values than the loudspeaker including the composite layer containing the powder of Comparative Example 1. This demonstrated that the composite layers containing the powders of Examples 14 to 17 exhibited excellent piezoelectric effects.
[0215] The improvement in sound pressure was due to the K contained in the powders of Examples 14 to 17. x Na (1-x) The crystallite size of the NbO3 particles is the same as that of the K powder in Comparative Example 1. x Na (1-x) It is believed that the superior piezoelectric performance was achieved because the crystallite size was larger than that of NbO3 particles. For example, when comparing Comparative Example 1 and Example 15, which have similar values of x (K / (K+Na)), the K contained in the powder of Example 15 is x Na (1-x) It can be seen that the crystallite size of the NbO3 particles calculated from the peak at 2θ=23.0±1.0° is larger than the crystallite size in the powder of Comparative Example 1.
[0216] Furthermore, as shown by the high value of the peak intensity ratio R, the powders of Examples 14 to 17 have K x Na (1-x) The fact that the material is of high quality and contains a large amount of NbO3 particles is also thought to have contributed to the excellent piezoelectric performance.
[0217] The configurations and combinations thereof in each embodiment are merely examples, and additions, omissions, substitutions, and other modifications of the configurations are possible without departing from the spirit of the present invention. Furthermore, the present invention is not limited to each embodiment, but is limited only by the scope of the claims. [Explanation of symbols]
[0218] 1...speaker, 10...film, 20...lower electrode, 30...composite layer, 40...upper electrode, 51, 52...O-rings, 61, 62...conductive tapes
Claims
1. K x Na (1-x) Nb y T (1-y) O 3 (wherein 0.16≦x≦0.77, 0.21≦y≦1), It has a cubic shape, The particle size is 0.1 μm or more and 100 μm or less, The crystal structure has an average crystallite size of 80 nm or more, determined from a peak at 2θ=23.0±1.0° of the niobate obtained by X-ray diffraction measurement; Niobate particles further comprising molybdenum.
2. The niobate particle of claim 1 , wherein the crystal structure comprises a perovskite crystal structure.
3. The niobate particles according to claim 1 or 2, wherein the crystal structure has an average crystallite size of 50 nm or more, determined from a peak at 2θ=32.0±1.2° of the niobate obtained by X-ray diffraction measurement.
4. Median diameter D calculated by laser diffraction / scattering method 50 The niobate particles according to claim 1 or 2, wherein the average particle diameter is 0.1 to 100 μm.
5. 3. The niobate particle according to claim 1, wherein the ratio (R) of the peak intensity I(100) of the peak at 2θ=23.0±1.0° to the peak intensity I(110) of the peak at 2θ=32.0±1.2° of the niobate, as determined by X-ray diffraction measurement, is 1 or more. R=I(100) / I(110)
6. The niobium content or the total content of niobium and tantalum in the niobate particles is determined by XRF analysis of the niobate particles, and is expressed as Nb 2 O 5 Conversion and Ta 2 O 5The niobate particles according to claim 1 or 2, wherein the total content in terms of mass converted is 50 to 99 mass%.
7. The potassium and / or sodium content in the niobate particles is determined by XRF analysis of the niobate particles, and is expressed as K 2 O equivalent and Na 2 The niobate particles according to claim 1 or 2, wherein the total content calculated as O is 0.5 to 40 mass%.
8. The molybdenum content in the niobate particles is determined by XRF analysis of the niobate particles, and is expressed as MoO 3 The niobate particles according to claim 1 or 2, wherein the content in terms of niobium is 0.01 to 20 mass%.
9. A method for producing the niobate particles according to claim 1, comprising the steps of: A method for producing niobate particles, comprising calcining a niobium compound, or a niobium compound and a tantalum compound, in the presence of a potassium compound and / or a sodium compound.
10. The method for producing niobate particles according to claim 9, wherein the sodium compound is sodium carbonate and the potassium compound is potassium carbonate.
11. 10. A method for producing the niobate particles according to claim 1 or 2, comprising calcining a niobium compound, or a niobium compound and a tantalum compound, in the presence of a molybdenum compound and a potassium compound and / or a sodium compound.
12. The method for producing niobate particles according to claim 11, wherein the molybdenum compound is at least one compound selected from the group consisting of molybdenum trioxide, potassium molybdate, and sodium molybdate.
13. The method includes a step of mixing a niobium compound or a niobium compound and a tantalum compound with a potassium compound and / or a sodium compound to obtain a mixture, and a step of calcining the mixture, The method for producing niobate particles according to claim 9 or 10, wherein the molar ratio (K+Na) / (Nb+Ta) of potassium atoms and sodium atoms to niobium atoms and tantalum atoms in the mixture is 1.1 or more.
14. The niobate particles according to claim 1 or 2, A resin composition comprising:
15. A molded article obtained by molding the resin composition according to claim 14.
Citation Information
Patent Citations
Piezoelectric element and piezoelectric element sheet
JP2020145408A
Composite filler, resin composition containing the same, high polymer composite piezoelectric body, and piezoelectric device, as well as manufacturing method of composite filler
JP2022012827A