SnZn solder and its manufacturing method
The SnZn alloy with trace elements and ammonium chloride hydrate enhances bonding strength and reduces costs, addressing the weaknesses of conventional lead-free solders on solar cell and liquid crystal substrates.
Patent Information
- Application Number
- JP2021532789
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-06-16
- Filing Date
- 2020-07-04
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-07-04
AI Technical Summary
Conventional lead-free solders are weaker and more expensive than tin-lead solder, making them unsuitable for applications requiring strong bonding, especially on electrodes like those found in solar cell and liquid crystal substrates.
A SnZn alloy is developed by adding trace amounts of P, In, Bi, and Sb as main materials and optional auxiliary materials like Al, Si, Ag, Cu, and Ni, maintaining or lowering the melting temperature while enhancing strength and adhesion, and using ammonium chloride hydrate powder to improve soldering adhesion.
The SnZn solder achieves strong bonding resistant to high and low temperatures, reduces melting temperature variation, and lowers production costs, while improving adhesion and electrical properties on electrodes.
Smart Images

Figure 0007572008000001 
Figure 0007572008000002 
Figure 0007572008000003
Abstract
Description
[Technical field]
[0001] The present invention relates to SnZn solder for use in solar cell substrates, liquid crystal substrates, etc., and to a method for producing the same. [Background technology]
[0002] Conventionally, tin-lead solder has been widely used for soldering lead wires to electrodes of solar cell substrates, liquid crystal substrates, etc., due to its high strength and low cost.
[0003] Furthermore, in the case of electrodes made of aluminum or the like, sufficient soldering strength could not be obtained, so silver paste was applied and sintered, and then the lead wire was soldered onto this with tin-lead solder.
[0004] Recently, there has been a growing demand for lead-free solder due to concerns about pollution. DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0005] Conventional lead-free solder has problems compared to tin-lead solder, such as its strength being slightly less than the required strength and its high price, preventing it from becoming an alternative. [Means for solving the problem]
[0006] The inventors have discovered that SnZn solder, a type of lead-free solder made of an alloy of Sn and Zn, is melted and alloyed by mixing in trace amounts of main materials such as P, In, Bi, Sb, etc. in total of 1 to 1.5 wt% or less, and if necessary, by mixing in trace amounts of secondary materials such as Al, Si, Ag, Cu, Ni, etc., resulting in a solder that is extremely strong on electrodes such as solar cell substrates and is resistant to repeated high and low temperature tests, and that the melting temperature of the SnZn solder remains roughly the same or is reduced even when these materials are mixed in.
[0007] Therefore, in the present invention, in SnZn solder consisting of an alloy of Sn and Zn, a main material containing one or more of P, In, Bi, and Sb is mixed into the base material, which is an alloy of Sn and Zn, in an amount of 1 to 1.5 wt% in total, and melted and alloyed.
[0008] In this case, the melting temperature of the SnZn solder after melting and alloying is set to be the same as or lower than the melting temperature of the base material.
[0009] The main material is alloyed within the skeleton of an alloy of Sn and Zn.
[0010] In addition, a secondary material containing one or more of Al, Si, Cu, Ag, and Ni, or a glass containing one or more of these, is mixed into the base material in an amount of 5 wt% or less as necessary, and melted and alloyed.
[0011] In addition, as the main material and the secondary material, an alloy of the main material and the secondary material is mixed into the base material and melted and alloyed.
[0012] In addition, the alloy of the main material and the secondary material is an alloy of Cu and P.
[0013] In addition, the base material, main material, and secondary material are mixed together or divided into several parts and then melted and alloyed.
[0014] It is also used for soldering lead wires to electrodes on solar cell substrates and liquid crystal substrates.
[0015] In addition, ammonium chloride hydrate powder or powder containing ammonium chloride hydrate is mixed into the SnZn solder at a concentration of 3 wt% or less to 0.05 wt% or more, which decomposes when heated for soldering, improving the solder adhesion to the object to be soldered. Effect of the Invention
[0016] As described above, in the present invention, by mixing a small amount of a main material containing one or more of P, In, Bi, Sb, etc., in a total of 1 to 1.5 wt% or less into a base material which is an alloy of Sn and Zn, and, as necessary, a small amount of a secondary material containing one or more of Al, Si, Cu, Ag, Ni, etc., or glass containing one or more of these, and melting and alloying them, a solder that is extremely strong for electrodes of solar cell substrates, etc. and can withstand repeated high and low temperature tests, and even when mixed, the melting temperature of SnZn solder remains almost the same or is lower, making it possible to manufacture it more cheaply.
[0017] In addition, the melting temperature of the SnZn solder after melting and alloying was the same as or lower than that of the base material, eliminating the rise in melting temperature caused by contamination.
[0018] In addition, the main material was alloyed within the skeleton of the Sn-Zn alloy, eliminating the adverse effect of precipitation.
[0019] In addition, by mixing one or more of Al, Si, Cu, Ag, Ni, etc., or glass containing one or more of these elements, and melting and alloying it to produce SnZn solder, it is possible to improve electrical properties such as the contact potential of the soldered object.
[0020] In addition, by manufacturing SnZn solder by mixing the main material and the secondary material, melting and alloying them, the main material was stabilized and the solder was made resistant to repeated high and low temperature tests.
[0021] In addition, by mixing ammonium chloride hydrate powder or powder containing ammonium chloride hydrate into the SnZn solder prepared, at a concentration of 3 wt% or less to 0.05 wt% or more, the powder decomposes when heated for soldering, improving the solder adhesion to the object to be soldered. Example 1
[0022] FIG. 1 is an explanatory diagram of the solder manufacturing method of the present invention.
[0023] FIG. 1(a) shows a flow chart, and FIG. 1(b) shows example materials.
[0024] In (a) of Fig. 1, S1 prepares the base material, main material, and secondary material. This is done by preparing the following materials shown in the material examples in (b) of Fig. 1.
[0025] Base material: Sn91 Zn9 ·Main material: P, In, Bi, Sb ·Auxiliary materials: Al, Si, Cu, Ag, Ni Here, the base material is the basic material (base material) of the SnZn alloy that forms the SnZn solder of the present invention, and here, Sn is 91wt%. Zn was used in the prototype at 9wt%. The weight ratio of Sn and Zn can be any within the range that allows the alloy to be created, for example, Zn can be 1 to 15wt%, and the remainder can be Sn (the ratio can be appropriately selected by experiment using the melting temperature as a guide).
[0026] The main material is a material that affects soldering such as oxide film removal, adhesion, wettability, fluidity, and viscosity on the surface of the soldered object during soldering, and in the present invention, the total amount of the main material is 1 to 1.5 wt% or less. Here, it is a material to be melted and alloyed by mixing one or more of P (oxide film removal and adhesion on the soldered object), In (wettability and fluidity), Bi (adhesion), and Sb (adhesion). The main material is a small amount of 1 to 1.5 wt% or less in total, and the melting temperature of the SnZn solder after mixing the main material with the base material and melting and alloying is equal to or slightly lower (for example, about 1 to 5°C lower) than the melting temperature of the base material. It is presumed that the main material enters the skeleton of the base material and reconstructs the skeleton because the total amount of the main material is a small amount of 1 to 1.5 wt% or less with respect to the base material.
[0027] The auxiliary material is a material added to the base material and the main material to improve the electrical properties (contact potential difference, contact resistance, IV characteristics in the case of solar cells, etc.) and adhesion of the soldered object (solar cell substrate, semiconductor substrate such as liquid crystal substrate, fired aluminum film, copper electrode, etc.), and here, the materials are Al (for fired aluminum film), Si (for silicon substrate), Cu (for copper electrode), Ag (for all), Ni (for silicon substrate with trace Ni plating), etc. As an auxiliary material, not only metals but also glasses containing metals may be added by mixing, melting, or alloying (oxygen and other gas components in glass are released to the outside during melting and alloying).
[0028] In S2, the main material and the secondary material are mixed into the base material prepared in S1.
[0029] In S3, the base material, main material, and secondary material are melted and alloyed. This is done by mixing the base material with the main material and secondary material in S2, heating and melting them, and stirring thoroughly to alloy them. In cases where the main material and secondary material are oxidized by oxygen in the air and alloying is difficult, inert gas (such as nitrogen gas) can be blown into the crucible as necessary, or a melting furnace or vacuum melting furnace filled with inert gas can be used.
[0030] S4 is the completed solder material (ABS-S).
[0031] As described above, the base material, main material, and secondary material are prepared, mixed, melted, and alloyed, making it possible to manufacture the SnZn solder (ABS-S) according to the present invention. The details will be described below in order.
[0032] FIG. 2 shows an explanatory diagram of the material manufacturing apparatus of the present invention.
[0033] In FIG. 2, the solder material 1 is the base material, main material, and secondary material prepared in S1 of FIG. 1 already described, and in this case is pieces (coarsely crushed) of metal, glass, or the like.
[0034] The solder material input tray 2 is used to place the solder material 1 thereon and input it into the melting furnace 3 .
[0035] The melting furnace 3 is heated by a heater 4 or the like, and the solder material 1 is put inside, where the base material, main material, and auxiliary material are melted and stirred to form an alloy. The melting furnace 3 is usually operated in the atmosphere, where the base material, main material, and auxiliary materials put inside are melted and stirred to form an alloy. During this process, an inert gas (such as nitrogen gas) is blown in as necessary to reduce oxidation caused by oxygen in the air, and the furnace is further sealed and filled with an inert gas (or evacuated) as necessary.
[0036] As described above, the base material, main material, and secondary material prepared in S1 of FIG. 1 are mixed, melted in the melting furnace 3, and alloyed by stirring, making it possible to manufacture the SnZn solder of the present invention.
[0037] FIG. 3 is an explanatory diagram of soldering of lead wires according to the present invention.
[0038] FIG. 3(a) shows a flow chart, and FIG. 3(b) shows an example of board / lead wiring.
[0039] In (a) of Fig. 3, S11 is ultrasonic pre-soldering of the solder (ABS-S) to the substrate pattern. For example, the SnZn solder of the present invention (the SnZn solder manufactured in S4 of Fig. 1) is supplied to the tip of an ultrasonic soldering iron to melt the portion (pattern) to be soldered to the electrode of a solar cell substrate, and ultrasonic waves are applied to solder the portion of the pattern on the substrate in advance (called ultrasonic pre-soldering).
[0040] In step S12, the lead wires are ultrasonically soldered or ultrasonically soldered. In step S11, the lead wires are placed along the portion (pattern) of the electrode of the solar cell substrate that has been ultrasonically pre-soldered in advance, and the SnZn solder of the present invention is melted to solder the lead wires while applying ultrasonic waves from above or without applying ultrasonic waves. When the SnZn solder has been pre-soldered in advance to the lead wires, it is not necessary to supply solder.
[0041] As described above, since it is difficult to solder the parts to be soldered (for example, the electrode parts of a solar cell substrate) using normal soldering, pre-soldering with the SnZn solder of the present invention is performed using ultrasound (S11), and then the lead wiring is ultrasonically soldered or ultrasonically soldered (S12) using the SnZn solder of the present invention on the parts (patterns) where pre-soldering has been performed.In this way, it is possible to ultrasonically pre-solder the electrode parts of a solar cell substrate that cannot be soldered using conventional methods, and then ultrasonically solder the lead wiring on top of that.
[0042] Furthermore, ultrasonic soldering is performed at a power of 10 W or less, usually 2 to 3 W. A strong power can damage the film (such as a nitride film) formed on the solar cell substrate and the crystals on the surface of the substrate, so it is not made too strong.
[0043] FIG. 3(b) shows an example of board / lead connections.
[0044] In Fig. 3(b), the substrate is an Al, Si substrate, glass substrate, etc., which are examples of substrates that are extremely difficult to solder using normal soldering. The SnZn solder of the present invention is ultrasonically pre-soldered to the electrode portions (patterns) of these substrates. Then, by ultrasonically soldering or non-ultrasonic soldering the lead wires to the pre-soldered portions (patterns), it becomes possible to solder the lead wires to the substrate.
[0045] The lead connection is a lead formation in which the SnZn solder of the present invention is used to solder to the electrode portion (pattern) on the board, and may be a wire (a circular copper wire solder-plated with the SnZn solder of the present invention; it is easier to solder if it is crushed into a slight oval), a ribbon (a thin copper sheet cut into a ribbon about 1 mm wide, which is solder-plated in advance with the SnZn solder of the present invention), etc.
[0046] FIG. 4 shows an explanatory diagram of soldering according to the present invention.
[0047] FIG. 4(a) shows an example of pre-soldering, and FIG. 4(b) shows an example of ribbon or wire soldering.
[0048] In FIG. 4(a), a silicon substrate 11 is an example of a solar cell substrate, and an aluminum sintered film 12 is formed on the entire back surface of the silicon substrate 11, for example.
[0049] The aluminum sintered film 12 is an electrode (aluminum sintered film) formed by applying aluminum paste (or screen printing in a predetermined pattern) to the entire back surface of the illustrated silicon substrate 11, which is a solar cell substrate, and sintering it.
[0050] The ultrasonic soldering iron tip 13 is a soldering iron tip that is heated while ultrasonic waves are applied thereto from an ultrasonic generator (not shown).
[0051] Solder (ABS-S) 14 is the SnZn solder of the present invention (the SnZn solder produced in S4 in FIG. 1).
[0052] Next, the soldering operation will be described.
[0053] (1) The silicon substrate 11 is transported onto a preheating table, fixed thereon by vacuum suction, and preheated (for example, to about 180° C.).
[0054] (2) Solder 14 is automatically supplied to the tip 13 of the ultrasonic soldering iron shown in the figure from the start point to the end point of the electrode pattern (strip-shaped pattern) to be formed on the aluminum sintered film 12, and while melting it, ultrasonic waves are applied and the iron is moved at a constant speed while being close enough to the aluminum sintered film 12 but not scraping it, thereby forming a strip-shaped preliminary solder pattern on the aluminum sintered film 12.
[0055] As a result of the above, it becomes possible to solder the SnZn solder 14 of the present invention onto the aluminum sintered film 12 in a predetermined preliminary solder pattern.
[0056] FIG. 4(b) shows an example of soldering a ribbon or wire.
[0057] In FIG. 4(b), an ultrasonic soldering iron tip 13-1 is a soldering iron tip that is heated with or without application of ultrasonic waves from an ultrasonic generator (not shown).
[0058] The soldered ribbon or wire 15 is a ribbon or wire that has been pre-soldered with the SnZn solder of the present invention. The wire 15 has better solderability if it is slightly deformed into an oval shape.
[0059] Next, the soldering operation of the ribbon or wire to the preliminary solder pattern portion will be described.
[0060] (1) As in FIG. 4(a), the silicon substrate 11 is preheated.
[0061] (2) The soldered ribbon or wire 14 is arranged along the preliminary solder pattern portion formed on the aluminum sintered film 12 on the upper (back) surface of the silicon substrate 11, and the soldered ribbon or wire 15 is lightly pressed from above with the tip 13-1 of an ultrasonic or non-ultrasonic soldering iron while being moved at a constant speed to the right as shown in the figure, melting the solder of the soldered ribbon or wire 15 and soldering it to the preliminary solder pattern portion.
[0062] As a result of the above, it becomes possible to solder the ribbon or wire 15 to which the SnZn solder 14 of the present invention has been pre-soldered, to the pre-solder pattern portion on the aluminum sintered film 12 .
[0063] The quality of the soldering with or without ultrasonic waves of the present invention is determined by soldering a ribbon or wire to the part to be soldered with or without ultrasonic waves, and pulling the ribbon or wire with a force slightly weaker than the force that would crack the board or the like. If it does not peel off from the board or the like, it is judged as good, and if it does peel off, it is judged as bad.
[0064] FIG. 5 shows an example of the composition of the solder of the present invention (ABS-S).
[0065] In FIG. 5, the base material, main material, and secondary material are the same as those described in FIG.
[0066] The composition examples are composition examples of the base material, main material, and secondary material.
[0067] The wt% examples are examples of the wt% compositions of the base material, main material, and secondary material.
[0068] The wt% ranges are examples of the wt% ranges of the composition of the base material, main material, and secondary material.
[0069] The compositions, examples of wt% and wt% ranges are shown in FIG.
[0070] Base material Main material Secondary material Composition example SnZn alloy P In Bi Al Si Cu Ag wt% example Sn Zn CuP8 In Bi Al Si Cu Ag 91 9 0.3 0.3 0.3 0.3 0.3 0.3 0.3 wt% range 99-85 1-15 Trace -0.1(P) 0.1-1.0 Trace -0.5 Each 5Wwt or less As an example of the composition, the prototype used a base material with 91 wt% Sn and 9 wt% Zn as shown in the figure. The composition range may be as long as it is stable within the range in which the SnZn alloy can be produced, for example, 1 to 15 wt% Zn, with the remainder being Sn, and may be determined through experiments by measuring the melting temperature of the produced SnZn base material.
[0071] The main materials include P, In, Bi, Sb, etc., but for P, P (red phosphorus) and CuP8 alloy (an alloy of 8 wt% P and the remainder Cu, copper phosphide where the wt% of P is 8% of CuP8) were used in the prototype. In addition, when about 0.1 wt% P (red phosphorus) was added (P saturated state), and when P in CuP8 was added as the main material, it was necessary to add a large amount of about 0.16 wt% (P saturated state). In the case of P, it is saturated at about 0.1 wt% (or about P = 0.16 wt% in the case of CuP8), and if it is added further, it becomes supersaturated, and the viscosity of SnZn solder increases significantly. Therefore, for normal use to ensure fluidity and wettability, it is desirable to add P below saturation. In the case of P, a very small amount (a small amount of about 0.001 wt%) is sufficient. Also, P saturation or supersaturation can be used appropriately depending on the application. Similarly, the same tendency is observed for other main materials, so the optimum amount to be added can be determined by experiment as necessary.
[0072] The total amount of the main material was preferably 1 to 1.5 wt% or less. The SnZn solder of the present invention, which is made by mixing, melting, and alloying a total amount of 1 to 1.5 wt% of the main material with a base material (Sn 91 wt%, Zn 9 wt%), has been measured to have a melting temperature that is the same as or 1 to 5°C lower than the melting temperature of the base material (for example, around 195°C). This is presumed to be because the total amount of the main material, 1 to 1.5 wt% or less, is incorporated into the skeleton of the base material (SnZn alloy) and the skeleton is reconstructed, resulting in the melting temperature being the same as or lower than that of the base material. This is also presumed to be because a mesh-like skeleton appears during mixing, melting, and alloying in a crucible, and when this is stirred and melted as a whole, it becomes a uniform alloy.
[0073] In addition, since solar cell substrates, liquid crystal substrates, etc. have silicon and an aluminum sintered film on the silicon, secondary materials such as Si, Al, Cu (copper wire, copper pattern, etc.), Ag (sintered electrode), and Ni (nickel plating on the silicon surface) are added taking into consideration these, and they improve the electrical characteristics (contact potential difference, contact resistance, and in the case of solar cells, IV characteristics, etc.) and the bonding strength, etc.
[0074] Fig. 6 shows a prototype of the solder of the present invention. The illustration shows examples of the many prototypes that can be used for the soldering of Fig. 4 described above. Unusable ones are omitted.
[0075] In FIG. 6, the base material of the SnZn solder of the present invention (the SnZn solder produced in S4 in FIG. 1) contains 91 wt % Sn and 9 wt % Zn.
[0076] The secondary materials used were Al and Si (others omitted).
[0077] The main materials used were metal materials In, Bi, and P (red phosphorus). CuP8 was copper phosphide with 8wt% P and the remainder Cu. As mentioned above, when using CuP8, the amount of P added had to be equivalent to 0.16wt% in order to saturate (P (red phosphorus) was saturated at 0.1wt%).
[0078] The sample number is the number of the sample produced.
[0079] For the above prototype sample numbers, only good ones were listed after ultrasonic soldering and non-ultrasonic soldering as shown in Figure 5. Those that could not be soldered were omitted.
[0080] 7 is an explanatory diagram of the TC test of the solder of the present invention. The sample used in the TC test was the sample No. "A-14" in FIG. 6 described above.
[0081] Figure 7(a) shows a schematic example of a TC test of ABS-S solder (A-14). At present, the TC test has exceeded 1000 hours (and is still ongoing).
[0082] Figure 7(b) shows an example of a sample photograph. As shown in the figure, a copper wire was soldered (ultrasonic soldering or scratched soldering) to an aluminum plate, a silicon surface, and an aluminum surface using A-14.
[0083] FIG. 7(c) shows an example of temperature conditions for the TC test. As shown in the figure, Maximum temperature is 87.5℃ -Minimum temperature is -24,4℃ Maximum humidity is 98.3% Minimum humidity is 1.6% The TC test was carried out under the following conditions.
[0084] Figure 7(d) shows an example of the test environment and results. As shown in the figure, (1) The test period is from May 1 to June 12, 2019 (1,000 hours). (2) Join the copper wire to the aluminum plate, silicon plate, and aluminum surface with solder A-14. (3) The high temperature condition is a high temperature furnace at 80°C. After placing the sample in the furnace, the temperature is increased.
[0085] (4) For low temperature conditions, place in a freezer at -20°C.
[0086] (5) When replacing the sample, replace it immediately without leaving it at room temperature.
[0087] The test results showed that the solder did not crumble and there were no problems.
[0088] As a result of carrying out a 1000-hour TC test under the above test conditions, sample No. "A-14" passed the test.
[0089] FIG. 8 shows an example of a TC test of the solder (A-14) of the present invention.
[0090] 8, the horizontal axis represents elapsed time (h), and the vertical axis represents temperature (° C.) / humidity (%), with the upper graph representing humidity and the lower graph representing temperature.
[0091] In Figure 8, the temperature graph at the bottom of the graph is The high temperature (maximum temperature) is 87.6°C as shown in (c) of Figure 7. The lowest temperature (minimum temperature) is -24.4°C as shown in (c) of Figure 7. and shows the record up to 1000 hours.
[0092] In Figure 8, the humidity graph at the top of the graph is The maximum humidity is 98.3% as shown in Figure 7(c). The minimum humidity is 1.6% as shown in FIG. 7(c). and shows the record up to 1000 hours.
[0093] FIG. 9 shows an ultrasonic (rubbing) / paste example of the present invention. "Paste / Ultrasonic (rubbing)" is a distinction between "soldering with ultrasonic", "rubbing the object with the tip of the soldering iron without ultrasonic", "using ammonium chloride (NH4Cl) hydrate paste (3wt% or less, 0.05wt% or more)", "using ammonium chloride anhydride paste (3wt% or less, 0.05wt% or more)", and "using resin (rosin) paste (3wt% or less, 0.05wt% or more)" when soldering to an object to be soldered using the SnZn solder of this invention.
[0094] The object to be soldered is the material to be soldered using the SnZn solder of the present invention, and is classified into Si (wafer, approximately 0.2 mm thick), Al sintered film sintered on a wafer, Cu (0.1 mm thick plate), Al (0.1 mm thick plate), and stainless steel (0.1 mm thick plate).
[0095] ·◎ indicates that the SnZn solder of the present invention has excellent adhesion to the soldering target (adhesion is judged to be excellent when a silicon wafer is broken when a tin-plated wire of 0.4 mmφ is soldered and pulled).
[0096] ·◯ indicates that the SnZn solder of the present invention has good adhesion to the soldering object (good adhesion is determined when a 0.4 mmφ tin-plated wire is soldered and pulled with a force that cracks the silicon wafer or a force (tensile strength) that is slightly weaker).
[0097] ·△ indicates that the SnZn solder of the present invention has poor adhesion to the object to be soldered (when a tin-plated wire of 0.4 mmφ is soldered and pulled, it immediately peels off).
[0098] ·× indicates poor adhesion of the SnZn solder of the present invention to the object to be soldered.
[0099] From the experiment shown in Figure 9 above, it was found that sufficient soldering strength could be obtained for Si wafers, Al sintered film, Cu, Al, and stainless steel when "with ultrasonic waves" and "rubbing the object to be soldered with the tip of the soldering iron without ultrasonic waves."
[0100] Furthermore, it was found that sufficient solder strength was obtained in the case of Cu and Al when ammonium chloride hydrate (3wt% or less, 0.05wt% or more) was used.
[0101] Furthermore, it was found that sufficient soldering strength was obtained in the case of Cu when resin (rosin) (3wt% or less, 0.05wt% or more) was used.
[0102] The powder-mixed SnZn solder of the present invention used in the experiment is prepared by drilling a hole (about 1-3 mm) or making a cut in the center of a thick rod-shaped solder, putting a predetermined amount of powder (e.g., ammonium chloride hydrate or resin powder) inside the hole or cut, and repeatedly rolling it out into a thin rod shape with a rolling roller (with grooves) several times, and finally processing (rolling) it into a solder filament of about 1 mmφ or 1 mm square. The powder put in (mixed in) can be observed near the center of the cross section of this solder filament. Then, the solder filament is melted while heating it by placing the tip of the soldering iron against the object to be soldered (e.g., a Cu plate, etc., if necessary, placed on a preheating table (e.g., 180°C)), and the powder mixed in the solder filament (e.g., ammonium chloride hydrate powder) is decomposed to try to significantly improve the adhesion to the part to be soldered (for example, in the case of a Cu plate, the adhesion was significantly improved. See Figure 9). [Brief description of the drawings]
[0103] [Figure 1] FIG. 2 is an explanatory diagram of the solder manufacturing method of the present invention. [Diagram 2] FIG. 2 is an explanatory diagram of a solder material manufacturing apparatus according to the present invention. [Diagram 3] FIG. 4 is an explanatory diagram of soldering of lead wires according to the present invention. [Figure 4] FIG. 2 is an explanatory diagram of soldering according to the present invention. [Diagram 5] 2 is an example of the composition of the solder of the present invention (ABS-S). [Figure 6] 1 is a prototype example of the solder of the present invention. [Figure 7] FIG. 2 is an explanatory diagram of a TC test of the solder of the present invention. [Figure 8] This is a TC test example of the solder (A-14) of the present invention. [Figure 9] This is an ultrasonic (rubbing) / paste example of the present invention. [Explanation of symbols]
[0104] 1: Solder material 2: Solder material tray 3: Melting furnace 4: Heater 11: Silicon substrate 12: Aluminum sintered film 13: Ultrasonic soldering iron tip 13-1: Soldering iron tip with or without ultrasonic 14: Solder 15: Soldered ribbon or wire
Claims
1. A SnZn solder is produced by mixing a main material consisting of P and two or more of In, Bi and Sb into a base material which is an alloy of Sn and Zn in a total amount of 1.0 wt% or less, which is a ratio relative to 100 wt% of the base material which is an alloy of Sn and Zn, and melting and alloying the main material, the main material being 1.0 wt% or less, the ratio being relative to 100 wt% of the base material which is an alloy of Sn and Zn, the SnZn solder being characterized in that the solder has improved oxide film removal, adhesion, fluidity and viscosity compared to the base material, and the melting temperature of the SnZn solder after melting and alloying is made the same as or lower than the melting temperature of the base material, thereby preventing the melting temperature from becoming higher than the melting temperature of the base material.
2. The SnZn solder according to claim 1, characterized in that a secondary material consisting of one or more of Al, Si, Cu, Ag, and Ni is mixed into the base material at a ratio of 5 wt% or less relative to 100 wt% of the base material, SnZn alloy, and melted and alloyed.
3. It is characterized by being used for soldering lead wires to electrodes of solar cell substrates or liquid crystal substrates. The SnZn solder according to claim 1 or 2.
4. 4. SnZn solder according to any one of claims 1 to 3, wherein ammonium chloride hydrate powder or, in the case of a powder containing ammonium chloride hydrate, the ammonium chloride hydrate is mixed in an amount of 3 wt% or less to 0.05 wt% or more relative to 100 wt% of the SZn solder, and wherein, when the SnZn solder is heated for soldering, the ammonium chloride hydrate decomposes, improving the solder adhesion to an object to be soldered compared to SnZn solder not containing ammonium chloride hydrate.
5. A method for producing SnZn solder, which comprises mixing a main material consisting of P and two or more of In, Bi and Sb into a base material which is an alloy of Sn and Zn in a total amount of 1.0 wt% or less, which is a ratio relative to 100 wt% of the base material which is an alloy of Sn and Zn, and melting and alloying the main material, characterized in that oxide film removal, adhesion, fluidity and viscosity are improved compared to the base material, and the melting temperature of the SnZn solder after melting and alloying is made the same as or lower than the melting temperature of the base material, thereby preventing it from becoming higher than the melting temperature of the base material.
6. A method for producing SnZn solder as described in claim 5, characterized in that a secondary material made of glass containing one or more of Al, Si, Cu, Ag, and Ni is mixed into the base material in an amount of 5 wt% or less, where the total content of each of the elements Al, Si, Cu, Ag, and Ni contained in the secondary material is 5 wt% or less relative to 100 wt% of the base material SnZn alloy, and then melted and alloyed.
7. 7. The method for producing SnZn solder according to claim 6, wherein the main material and the secondary material are alloys of the main material and the secondary material, which are mixed into the base material and melted and alloyed.
8. 8. The method for producing SnZn solder according to claim 7, wherein the alloy of the main material and the sub-material is an alloy of Cu and P.
9. 9. The method for producing SnZn solder according to claim 6, wherein the base material, main material, and auxiliary material are mixed together or in a plurality of parts, and then melted and alloyed.
10. A method for producing SnZn solder, comprising mixing ammonium chloride hydrate powder or, in the case of a powder containing ammonium chloride hydrate, the ammonium chloride hydrate contained therein into the SnZn solder according to any one of claims 5 to 9, in an amount of 3 wt% or less to 0.05 wt% or more, which is a ratio relative to 100 wt% of the SZn solder, and wherein, when the SnZn solder is heated for soldering, the ammonium chloride hydrate decomposes, improving the solder adhesion to the object to be soldered compared to SnZn solder not mixed with ammonium chloride hydrate.
Citation Information
Patent Citations
Lead-free solder for micro alloyed eutectic alloy of stannum and zinc
CN101092006A
Tin-zinc based leadless solder
JP1997155587A
Soldering material
JP2000015478A
Solder metal, solder paste, soldering method, soldered circuit board and soldered part
JP2002361476A
Lead-free soldering paste
JP2003010996A
Cited By
Low temperature solder, method for manufacturing low temperature solder, and low temperature solder-coated lead wire