Flame retardant foams and foam components
The flame-retardant foam with optimized density, compression load, and elongation properties, combined with non-halogen flame retardants, provides enhanced flame resistance, flexibility, and stress dispersion for electronic devices.
Patent Information
- Application Number
- JP2020070759
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-10
- Filing Date
- 2020-04-10
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-04-10
AI Technical Summary
Existing resin foams used in electronic devices lack high flame retardancy, flexibility, and stress dispersion properties, particularly when composed of thermoplastic polymers, and conventional flame retardants like bromine, chlorine, and antimony compounds pose environmental and handling issues.
A flame-retardant foam with a density of 0.02-0.40 g/cm³, 50% compression load of 0.5-8.0 N/cm², and elongation at break of 120% or less, incorporating a non-halogen-non-antimony flame retardant, such as magnesium hydroxide, with a cellular structure optimized for flexibility and stress dispersion.
The foam achieves high flame retardancy, excellent flexibility, and effective stress dispersion, addressing the limitations of conventional foams and flame retardants.
Smart Images

Figure 0007572157000002 
Figure 0007572157000001
Abstract
Description
[Technical field]
[0001] The present invention relates to flame retardant foams and foam components. [Background technology]
[0002] In recent years, there have been changes in the size of clearances in parts where resin foams or foam members are used, and there is a demand for products that can accommodate smaller clearances.
[0003] Resin foams and foamed materials are used to protect the screens and circuit boards of electronic devices. In recent years, electronic devices such as smartphones and laptops are increasingly used not only indoors but also outdoors when moving around, which makes them more susceptible to unexpected loads due to dropping the device or external pressure loads. Therefore, if such loads can be effectively dispersed, it is possible to prevent the destruction of electronic devices due to unexpected loads.
[0004] For this reason, there is a growing demand for resin foams and foam members that are highly flexible, can accommodate smaller clearances, and have a higher level of stress dispersion.
[0005] However, resin foams are made of thermoplastic polymers and therefore have the problem of being flammable. Electronic devices such as smartphones and laptops use heating elements such as batteries and various elements, which may ignite, making it essential to impart flame retardancy to them.
[0006] Conventionally, various flame retardants have been blended to impart flame retardancy. For example, bromine-based resins, chlorine-based resins, phosphorus-based compounds, antimony-based compounds, etc., are used as such flame retardants. However, there is a demand to avoid the use of these flame retardants as much as possible due to their handling properties and environmental impact, and flame retardants that do not contain these compounds have been recently considered. Metal hydroxides such as magnesium hydroxide and aluminum hydroxide are used as such flame retardants. However, flame retardants using these metal hydroxides are inferior in flame retardancy compared to conventional flame retardants such as bromine-based resins, chlorine-based resins, phosphorus-based compounds, and antimony-based compounds, and a large amount of compounding is required to impart the same flame retardancy as conventional flame retardants, resulting in a problem of inferior moldability.
[0007] In recent years, a method has been proposed for obtaining a foam having a fine cell structure, in which an inert gas is dissolved in a polymer under high pressure, and then the pressure is suddenly reduced to form a foam structure. For example, Patent Document 1 discloses a method in which a thermoplastic polymer is charged in a pressure vessel, a high-pressure gas is charged while heating the polymer to its softening point, and then the pressure is reduced to form bubbles.
[0008] However, although the foam described in Patent Document 1 is flexible to a certain extent, it does not have flame retardancy, and there is no disclosure or suggestion as to its stress dispersibility.
[0009] Patent Document 2 discloses a method for obtaining a highly foamed resin foam having excellent flame retardancy and flexibility by combining a metal hydroxide, which is used as an environmentally friendly flame retardant, with carbon black.
[0010] However, the resin foam described in Patent Document 2 does not exhibit sufficient flexibility, and there is no disclosure or suggestion as to stress dispersibility. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] Japanese Patent Application Publication No. 6-322168 [Patent Document 2] JP2003-165860A Summary of the Invention [Problem to be solved by the invention]
[0012] An object of the present invention is to provide a flame-retardant foam having high flame retardancy, excellent flexibility, and excellent stress dispersion properties, and to provide a foam member having such a flame-retardant foam as a flame-retardant foam layer. [Means for solving the problem]
[0013] The flame-retardant foam of the present invention is Apparent density is 0.02g / cm 3 ~0.40g / cm 3 and 50% compression load is 0.5N / cm 2 ~8.0N / cm 2 and The breaking elongation in a tensile test is 120% or less.
[0014] In one embodiment, the flame-retardant foam has an average cell diameter of 10 μm to 200 μm.
[0015] In one embodiment, the flame-retardant foam has a coefficient of variation of cell diameter of 0.5 or less.
[0016] In one embodiment, the flame-retardant foam has a cell ratio of 30% or more.
[0017] In one embodiment, the flame-retardant foam has a cell wall thickness of 0.1 μm to 10 μm.
[0018] In one embodiment, the flame retardant foam includes a flame retardant agent.
[0019] In one embodiment, the flame retardant comprises a non-halogen, non-antimony flame retardant.
[0020] In one embodiment, the flame retardant has a bulk density of 0.8 g / cm 3 The following is the result.
[0021] In one embodiment, the flame-retardant foam has a residue at 650° C. of 20% by weight or more.
[0022] In one embodiment, the resin constituting the flame-retardant foam is a polyolefin resin.
[0023] In one embodiment, the polyolefin-based resin is a mixture of a polypropylene other than a polyolefin-based elastomer and a polyolefin-based elastomer.
[0024] The foam material of the present invention has the above-mentioned flame-retardant foam as a flame-retardant foam layer, and has a pressure-sensitive adhesive layer on at least one side of the flame-retardant foam layer. Effect of the Invention
[0025] According to the present invention, it is possible to provide a flame-retardant foam having high flame retardancy, excellent flexibility, and excellent stress dispersion properties, and also to provide a foam member having such a flame-retardant foam as a flame-retardant foam layer. [Brief description of the drawings]
[0026] [Figure 1] FIG. 2 is a schematic cross-sectional view of a stress relaxation tester. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] ≪≪1. Flame-retardant foam≫≫ The flame-retardant foam of the present invention has an apparent density of 0.02 g / cm 3 ~0.40g / cm 3 and the 50% compression load is 0.5N / cm 2 ~8.0N / cm2 and the breaking elongation in a tensile test is 120% or less. Since the flame-retardant foam of the present invention has an apparent density, a 50% compression load, and a breaking elongation in a tensile test within the above ranges, the foam has high flame retardancy, excellent flexibility, and excellent stress dispersibility.
[0028] The flame-retardant foam of the present invention has a cell structure (cell structure). Examples of such a cell structure (cell structure) include a closed cell structure, an open cell structure, and a semi-open, semi-closed cell structure (a cell structure in which a closed cell structure and an open cell structure are mixed). In terms of being able to more effectively exhibit the effects of the present invention, the cell structure of the flame-retardant foam of the present invention is preferably an open cell structure or a semi-open, semi-closed cell structure, and more preferably a semi-open, semi-closed cell structure. When the cell structure of the flame-retardant foam of the present invention is a semi-open, semi-closed cell structure, the proportion of the closed cell structure therein is preferably 40% or less, more preferably 30% or less.
[0029] The closed cell ratio of the flame-retardant foam of the present invention can be determined, for example, by submerging a measurement object in water in an environment of a temperature of 23° C. and a humidity of 50%, measuring the mass thereafter, and then sufficiently drying the object in an oven at 80° C., and then measuring the mass again. In addition, since open cells can retain moisture, the mass of the open cells is measured and determined.
[0030] The flame-retardant foam of the present invention has an apparent density of 0.02 g / cm 3 ~0.40g / cm 3 and preferably 0.03 g / cm 3 ~0.30g / cm 3 and more preferably 0.04 g / cm 3 ~0.20g / cm 3 and particularly preferably 0.05 g / cm 3 ~0.15g / cm 3 and most preferably 0.07 g / cm 3 ~0.10g / cm 3When the apparent density is within the above range, the flame-retardant foam of the present invention can have higher flame retardancy, superior flexibility, and superior stress dispersibility. The method for measuring the apparent density will be described in detail later.
[0031] The flame-retardant foam of the present invention has a 50% compression load of 0.5 N / cm 2 ~8.0N / cm 2 and preferably 0.6 N / cm 2 ~6.0N / cm 2 and more preferably 0.7 N / cm 2 ~5.5N / cm 2 and particularly preferably 0.8 N / cm 2 ~5.0N / cm 2 and most preferably 0.9 N / cm 2 ~4.5N / cm 2 When the 50% compression load is within the above range, the flame-retardant foam of the present invention can have higher flame retardancy, superior flexibility, and superior stress dispersion. The method for measuring the 50% compression load will be described in detail later.
[0032] The flame-retardant foam of the present invention has a breaking elongation in a tensile test of 120% or less, preferably 110% or less, more preferably 105% or less, even more preferably 100% or less, particularly preferably 95% or less, and most preferably 90% or less. The lower limit of the breaking elongation in a tensile test of the flame-retardant foam of the present invention is preferably 1% or more, more preferably 5% or more, even more preferably 10% or more, particularly preferably 15% or more, and most preferably 20% or more. When the breaking elongation in a tensile test is within the above range, the flame-retardant foam of the present invention can have higher flame retardancy, excellent flexibility, and excellent stress dispersion. If the breaking elongation in a tensile test is small, the deformation of the cell walls of the flame-retardant foam when a load is applied to the flame-retardant foam is small. For example, when a filler is added, slippage is likely to occur at the interface between the resin constituting the flame-retardant foam and the filler, and the load can be further relaxed. On the other hand, if the breaking elongation in the tensile test is too large, the cell walls of the flame-retardant foam may be significantly deformed, making it difficult to relax the load. The method for measuring the breaking elongation in the tensile test will be described in detail later.
[0033] The flame-retardant foam of the present invention has an average cell diameter (average cell diameter) of preferably 10 μm to 200 μm, more preferably 15 μm to 180 μm, even more preferably 20 μm to 150 μm, particularly preferably 23 μm to 120 μm, and particularly preferably 25 μm to 100 μm. When the average cell diameter is within the above range, the flame-retardant foam of the present invention can have higher flame retardancy, excellent flexibility, and excellent stress dispersibility. In addition, the foam can have excellent compression recovery, and can return to nearly its original thickness in a short time after receiving an impact, so that the foam can have excellent resistance to repeated impacts. The method for measuring the average cell diameter will be described in detail later.
[0034] The flame-retardant foam of the present invention has a coefficient of variation of cell diameter (cell diameter) of preferably 0.5 or less, more preferably 0.48 or less, even more preferably 0.45 or less, particularly preferably 0.43 or less, and most preferably 0.4 or less. The lower limit of the coefficient of variation of cell diameter of the flame-retardant foam of the present invention is preferably 0.01 or more, more preferably 0.05 or more, even more preferably 0.1 or more, particularly preferably 0.15 or more, and most preferably 0.2 or more. When the coefficient of variation of cell diameter is within the above range, the flame-retardant foam of the present invention can have higher flame retardancy, excellent flexibility, and excellent stress dispersibility. The larger the coefficient of variation of cell diameter, the more stress is concentrated locally, so the smaller the coefficient of variation of cell diameter, the more preferable. The method for measuring the coefficient of variation of cell diameter will be described in detail later.
[0035] The flame-retardant foam of the present invention has a cell ratio (cell rate) of preferably 30% or more, more preferably 50% or more, even more preferably 65% or more, even more preferably 75% or more, particularly preferably 80% or more, and most preferably 90% or more. The upper limit of the cell ratio is practically 99% or less. By having the cell ratio within the above range, the flame-retardant foam of the present invention can have higher flame retardancy, excellent flexibility, and excellent stress dispersion. If the cell ratio is small, the repulsive stress when the flame-retardant foam is compressed becomes high, and when the flame-retardant foam is used in a gap in an equipment, the equipment may be damaged. The method for measuring the cell ratio will be described in detail later.
[0036] The flame-retardant foam of the present invention has a cell wall thickness of preferably 0.1 μm to 10 μm, more preferably 0.3 μm to 8 μm, even more preferably 0.5 μm to 5 μm, particularly preferably 0.7 μm to 4 μm, and most preferably 1 μm to 3 μm. When the cell wall thickness is within the above range, the flame-retardant foam of the present invention can have higher flame retardancy, excellent flexibility, and excellent stress dispersion. If the cell wall thickness is too thin, the flame-retardant foam may easily deform under load, and sufficient load dispersion effect may not be obtained. If the cell wall thickness is too thick, the flame-retardant foam may be difficult to deform under load, and may have poor step-following ability when used in the gap of equipment. The method for measuring the cell wall thickness will be described in detail later.
[0037] The flame-retardant foam of the present invention has a residue at 650° C. of preferably 20% by weight or more, more preferably 20% by weight to 80% by weight, even more preferably 22% by weight to 70% by weight, particularly preferably 26% by weight to 60% by weight, and most preferably 30% by weight to 50% by weight. The method for measuring the residue at 650° C. will be described in detail later.
[0038] The shape of the flame-retardant foam of the present invention may be any appropriate shape depending on the purpose. A typical example of such a shape is a sheet, and in this case, the flame-retardant foam of the present invention may be treated as a flame-retardant foam layer.
[0039] When the flame-retardant foam of the present invention has a sheet-like shape (i.e., when it has a flame-retardant foam layer), its thickness is preferably 30 μm to 5000 μm, more preferably 35 μm to 4000 μm, even more preferably 40 μm to 3000 μm, and particularly preferably 45 μm to 2500 μm. When the thickness of the flame-retardant foam layer is within the above range, the flame-retardant foam layer can easily follow even a minute clearance. In addition, when the thickness of the flame-retardant foam layer is within the above range, bubbles can be uniformly contained, and excellent impact absorption properties can be exhibited.
[0040] The flame-retardant foam of the present invention can be formed by any appropriate method as long as the effects of the present invention are not impaired. A representative example of such a method is a method of foaming a resin composition containing a resin material (polymer).
[0041] ≪1-1. Resin composition≫ The flame-retardant foam of the present invention can be typically obtained by foaming a resin composition. The resin composition contains a resin material (polymer).
[0042] As the resin material (polymer) contained in the resin composition, any appropriate resin material (polymer) can be adopted as long as it does not impair the effects of the present invention. Examples of such resin materials (polymers) include acrylic resins, silicone resins, urethane resins, polyolefin resins, ester resins, and rubber resins. Such resin materials (polymers) may be one type or two or more types.
[0043] The content of the resin material (polymer) in the resin composition is preferably 30 to 95% by weight, more preferably 35 to 90% by weight, further preferably 40 to 80% by weight, and particularly preferably 40 to 60% by weight. When the content of the resin material (polymer) in the resin composition is within the above range, the flame-retardant foam of the present invention can have higher flame retardancy, excellent flexibility, and excellent stress dispersion.
[0044] The resin material (polymer) contained in the resin composition is preferably a polyolefin resin, in that the effects of the present invention can be more effectively exhibited. The polyolefin resin may be one type only, or two or more types.
[0045] The content of polyolefin resin in the resin material (polymer) contained in the resin composition is preferably 50% by weight to 100% by weight, more preferably 70% by weight to 100% by weight, even more preferably 90% by weight to 100% by weight, particularly preferably 95% by weight to 100% by weight, and most preferably substantially 100% by weight.
[0046] The polyolefin resin is preferably at least one selected from the group consisting of polyolefins and polyolefin elastomers, and more preferably a combination of polyolefins and polyolefin elastomers.
[0047] When a polyolefin and a polyolefin elastomer are used in combination as the polyolefin resin, the content ratio of the polyolefin to the polyolefin elastomer (polyolefin / polyolefin elastomer) is, in terms of better exhibiting the effects of the present invention, preferably 1 / 99 to 99 / 1, more preferably 10 / 90 to 90 / 10, even more preferably 20 / 80 to 80 / 20, and particularly preferably 30 / 70 to 70 / 30, by weight.
[0048] The polyolefin may be used alone or in combination of two or more kinds.
[0049] The polyolefin elastomer may be of only one kind, or of two or more kinds.
[0050] In this specification, the term "polyolefin" does not include "polyolefin-based elastomers."
[0051] As the polyolefin, any appropriate polyolefin may be used as long as it does not impair the effects of the present invention. Examples of such polyolefins include linear polyolefins and branched (branched) polyolefins.
[0052] Such polyolefins include, for example, polymers constructed (formed) with α-olefins as an essential monomer component, i.e., polymers having at least a structural unit derived from α-olefins in the molecule (per molecule). Such polyolefins may be, for example, polymers constructed only from α-olefins, or may be polymers constructed from α-olefins and monomer components other than α-olefins.
[0053] The polyolefin may be a homopolymer or a copolymer containing two or more monomers. When the polyolefin is a copolymer, any suitable copolymer form may be adopted as the copolymer form. Examples of such copolymer forms include random copolymers and block copolymers.
[0054] As the α-olefin that can constitute the polyolefin, for example, an α-olefin having 2 to 8 carbon atoms (for example, ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, etc.) is preferable. The α-olefin that can constitute the polyolefin may be only one type or two or more types.
[0055] Examples of monomer components other than α-olefins that can constitute polyolefins include ethylenically unsaturated monomers such as vinyl acetate, acrylic acid, acrylic acid esters, methacrylic acid, methacrylic acid esters, vinyl alcohol, etc. The monomer components other than α-olefins that can constitute polyolefins may be one type or two or more types.
[0056] Specific examples of polyolefins include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, polypropylene (propylene homopolymer), copolymers of ethylene and propylene, copolymers of ethylene and an α-olefin other than ethylene, copolymers of propylene and an α-olefin other than propylene, copolymers of ethylene, propylene and an α-olefin other than ethylene and propylene, and copolymers of propylene and an ethylenically unsaturated monomer.
[0057] The polyolefin is preferably a polymer (polypropylene-based polymer) constituted with propylene as an essential monomer component, that is, a polymer having at least a structural unit derived from propylene, in terms of being able to more effectively exhibit the effects of the present invention. Examples of such polypropylene-based polymers include polypropylene (propylene homopolymer), copolymers of ethylene and propylene, and copolymers of propylene and an α-olefin other than propylene, and preferably polypropylene (propylene homopolymer). The polypropylene-based polymer may be one type only, or two or more types.
[0058] The melt flow rate (MFR) of the polyolefin at 230° C. is preferably 0.2 g / 10 min to 10 g / 10 min, more preferably 0.25 g / 10 min to 5 g / 10 min, further preferably 0.3 g / 10 min to 3 g / 10 min, and particularly preferably 0.35 g / 10 min to 1.5 g / 10 min, in order to more effectively exhibit the effects of the present invention. The melt flow rate (MFR) of the polyolefin at 230° C. refers to the MFR measured at a temperature of 230° C. and a load of 2.16 kgf according to ISO1133 (JIS-K-7210).
[0059] As the polyolefin, it is preferable to use two or more polyolefins having different melt flow rates (MFR) within the above range at a temperature of 230° C. in combination, in order to further exhibit the effects of the present invention. In this case, a polyolefin having a melt flow rate (MFR) at a temperature of 230° C. of preferably 0.2 g / 10 min or more and less than 0.7 g / 10 min (more preferably 0.2 g / 10 min to 0.65 g / 10 min) is used in combination with a polyolefin having a melt flow rate (MFR) at a temperature of 230° C. of preferably 0.7 g / 10 min to 10 g / 10 min (more preferably 0.7 g / 10 min to 5 g / 10 min, even more preferably 0.7 g / 10 min to 3 g / 10 min, particularly preferably 0.7 g / 10 min to 1.5 g / 10 min, and most preferably 0.7 g / 10 min to 1.3 g / 10 min).
[0060] When two or more polyolefins having different melt flow rates (MFR) at a temperature of 230° C. within the above range are used in combination as the polyolefin, for example, a polyolefin having a melt flow rate (MFR) at a temperature of 230° C. of preferably 0.2 g / 10 min or more and less than 0.7 g / 10 min (more preferably 0.2 g / 10 min to 0.65 g / 10 min) and a polyolefin having a melt flow rate (MFR) at a temperature of 230° C. of preferably 0.7 g / 10 min to 10 g / 10 min (more preferably 0.7 g / 10 min to 5 g / 10 min) are used in combination. The content ratio of the polyolefin (polyolefin copolymer) to the polyolefin copolymer (polyolefin copolymer) is preferably 1 / 99 to 99 / 1, more preferably 10 / 90 to 90 / 10, still more preferably 20 / 80 to 80 / 20, particularly preferably 30 / 70 to 70 / 30, and most preferably 40 / 60 to 60 / 40, in terms of a weight ratio, in order to further exhibit the effects of the present invention.
[0061] As the polyolefin, commercially available products may be used, such as "E110G" (manufactured by Prime Polymer Co., Ltd.), "EA9" (manufactured by Japan Polypropylene Corporation), "EA9FT" (manufactured by Japan Polypropylene Corporation), "E-185G" (manufactured by Prime Polymer Co., Ltd.), "WB140HMS" (manufactured by Borealis), and "WB135HMS" (manufactured by Borealis).
[0062] As the polyolefin-based elastomer, any suitable polyolefin-based elastomer may be adopted within the scope of not impairing the effects of the present invention. Examples of such polyolefin-based elastomers include so-called non-crosslinked thermoplastic olefin-based elastomers (TPOs) such as ethylene-propylene copolymers, ethylene-propylene-diene copolymers, ethylene-vinyl acetate copolymers, polybutene, polyisobutylene, chlorinated polyethylene, elastomers in which a polyolefin component and a rubber component are physically dispersed, and elastomers in which a polyolefin component and a rubber component have a microphase separation structure; dynamically crosslinked thermoplastic olefin-based elastomers (TPVs) which are multiphase polymers obtained by dynamically heat treating a mixture containing a resin component A (olefin-based resin component A) forming a matrix and a rubber component B forming a domain in the presence of a crosslinking agent, and which have a sea-island structure in which crosslinked rubber particles are finely dispersed as domains (island phases) in the resin component A which is a matrix (sea phase); and the like.
[0063] The polyolefin-based elastomer preferably contains a rubber component. Examples of such rubber components include those described in JP-A-08-302111, JP-A-2010-241934, JP-A-2008-024882, JP-A-2000-007858, JP-A-2006-052277, JP-A-2012-072306, JP-A-2012-057068, JP-A-2010-241897, JP-A-2009-067969, and JP-A-03 / 002654.
[0064] Specific examples of elastomers having a microphase-separated structure of a polyolefin component and an olefin-based rubber component include elastomers made of polypropylene resin (PP) and ethylene-propylene rubber (EPM), elastomers made of polypropylene resin (PP) and ethylene-propylene-diene rubber (EPDM), etc. From the viewpoint of compatibility, the weight ratio of the polyolefin component to the olefin-based rubber component (polyolefin component / olefin-based rubber) is preferably 90 / 10 to 10 / 90, more preferably 80 / 20 to 20 / 80.
[0065] Dynamically crosslinked thermoplastic olefin elastomers (TPV) generally have a higher elastic modulus and smaller compression set than non-crosslinked thermoplastic olefin elastomers (TPO), which gives them good recovery properties and allows them to show excellent recovery properties when foamed.
[0066] As described above, dynamically crosslinked thermoplastic olefin-based elastomers (TPVs) are obtained by dynamically heat treating a mixture containing a resin component A (olefin-based resin component A) that forms a matrix and a rubber component B that forms domains, in the presence of a crosslinking agent. These TPVs are multiphase polymers having an island-sea structure in which crosslinked rubber particles are finely dispersed as domains (island phases) in resin component A, which is the matrix (sea phase).
[0067] Examples of dynamically crosslinked thermoplastic olefin-based elastomers (TPVs) include those described in JP-A-2000-007858, JP-A-2006-052277, JP-A-2012-072306, JP-A-2012-057068, JP-A-2010-241897, JP-A-2009-067969, and JP-A-03 / 002654.
[0068] As the dynamically crosslinked thermoplastic olefin-based elastomer (TPV), commercially available products may be used, such as "Zeotherm" (manufactured by Zeon Corporation), "Thermorun" (manufactured by Mitsubishi Chemical Corporation), and "Sarlink 3245D" (manufactured by Toyobo Co., Ltd.).
[0069] The melt flow rate (MFR) of the polyolefin elastomer at a temperature of 230° C. is preferably 2 g / 10 min to 15 g / 10 min, more preferably 3 g / 10 min to 10 g / 10 min, further preferably 3.5 g / 10 min to 9 g / 10 min, particularly preferably 4 g / 10 min to 8 g / 10 min, and most preferably 4.5 g / 10 min to 7.5 g / 10 min, in order to further exhibit the effects of the present invention. The melt flow rate (MFR) of the polyolefin elastomer at a temperature of 230° C. refers to the MFR measured at a temperature of 230° C. and a load of 2.16 kgf according to ISO1133 (JIS-K-7210).
[0070] The melt tension (190° C., at break) of the polyolefin elastomer is preferably less than 10 cN, and more preferably from 5 cN to 9.5 cN, in order to more effectively exert the effects of the present invention.
[0071] The JIS A hardness of the polyolefin elastomer is preferably 30° to 95°, more preferably 35° to 90°, even more preferably 40° to 88°, particularly preferably 45° to 85°, and most preferably 50° to 83°, in order to further exert the effects of the present invention. The JIS A hardness refers to the hardness measured based on ISO7619 (JIS K6253).
[0072] The resin composition preferably contains a flame retardant in order to further exert the effects of the present invention. The resin composition may contain only one type of flame retardant or two or more types of flame retardants.
[0073] The content of the flame retardant in the resin composition is preferably 10 to 70% by weight, more preferably 15 to 65% by weight, further preferably 20 to 60% by weight, and particularly preferably 40 to 60% by weight. When the content of the flame retardant in the resin composition is within the above range, the flame-retardant foam of the present invention can have higher flame retardancy, excellent flexibility, and excellent stress dispersion.
[0074] Examples of flame retardants that can be included in the resin composition include bromine-based flame retardants, chlorine-based flame retardants, phosphorus-based flame retardants, and antimony-based flame retardants. However, chlorine-based flame retardants and bromine-based flame retardants generate gas components that are harmful to the human body and corrosive to equipment when burned, and phosphorus-based flame retardants and antimony-based flame retardants have problems such as toxicity and explosiveness. Therefore, in the present invention, non-halogen-non-antimony flame retardants are preferred as flame retardants that can be included in the resin composition.
[0075] The non-halogen-non-antimony flame retardant is a compound containing at least one selected from the group consisting of aluminum, magnesium, calcium, nickel, cobalt, tin, zinc, copper, iron, titanium and boron, which can further exert the effects of the present invention. Representative examples of such inorganic compounds include hydrated metal compounds such as aluminum hydroxide, magnesium hydroxide, hydrates of magnesium oxide and nickel oxide, and hydrates of magnesium oxide and zinc oxide. The hydrated metal compounds may be surface-treated.
[0076] The bulk density of the flame retardant that can be contained in the resin composition can be any appropriate bulk density as long as it does not impair the effects of the present invention. In order to further exhibit the effects of the present invention, the bulk density is preferably 0.8 g / cm. 3 More preferably, it is 0.6 g / cm or less. 3 or less, and more preferably 0.4 g / cm 3 or less, and particularly preferably 0.35 g / cm 3 Below 0.3 g / cm, most preferably 0.3 g / cm3 The lower limit of bulk density is practically 0.01 g / cm 3 or more, preferably 0.05 g / cm 3 More preferably, it is 0.1 g / cm 3 That is all. If the bulk density of the flame retardant that can be contained in the resin composition is within the above range, sufficient flame retardancy can be imparted even if the amount of the flame retardant used is small. If the amount of the flame retardant used can be reduced, a flame-retardant foam that is highly expanded, flexible, and has excellent stress dispersion properties can be obtained. In addition, if the bulk density of the flame retardant that can be contained in the resin composition is too high, the dispersibility of the flame retardant in the resin composition may be deteriorated, and the flame retardancy of the flame-retardant foam may vary or the appearance quality of the flame-retardant foam may be impaired.
[0077] As the particle diameter of the flame retardant that can be contained in the resin composition, any appropriate particle diameter can be adopted as long as the effect of the present invention is not impaired. Such a particle diameter is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less, in terms of being able to further express the effect of the present invention. The lower limit of the particle diameter of the flame retardant that can be contained in the resin composition is practically 0.1 μm or more. If the particle diameter of the flame retardant that can be contained in the resin composition is within the above range, the dispersibility of the flame retardant in the resin composition can be improved, so that the flame retardancy of the flame retardant foam can be uniformly expressed and the appearance quality of the flame retardant foam can be maintained. If the particle diameter of the flame retardant that can be contained in the resin composition is too high, the dispersibility of the flame retardant in the resin composition may be deteriorated, and the flame retardancy of the flame retardant foam may vary or the appearance quality of the flame retardant foam may be impaired. In addition, if the particle diameter of the flame retardant that can be contained in the resin composition is too high, the load dispersibility of the flame retardant foam may be reduced.
[0078] The specific surface area of the flame retardant that can be contained in the resin composition can be any appropriate specific surface area as long as it does not impair the effects of the present invention. In terms of being able to more effectively exhibit the effects of the present invention, the specific surface area is preferably 2 m 2 / g or more, more preferably 4m 2 / g or more, more preferably 6m 2The upper limit of the specific surface area of the flame retardant that can be contained in the resin composition is practically 20 m 2 / g or less. If the specific surface area of the flame retardant that can be contained in the resin composition is within the above range, the dispersibility of the flame retardant in the resin composition can be improved, so that the flame retardancy of the flame retardant foam can be uniformly expressed and the appearance quality of the flame retardant foam can be maintained. If the specific surface area of the flame retardant that can be contained in the resin composition is too high, the dispersibility of the flame retardant in the resin composition may be deteriorated, and the flame retardancy of the flame retardant foam may vary or the appearance quality of the flame retardant foam may be impaired. In addition, if the specific surface area of the flame retardant that can be contained in the resin composition is too high, the load dispersibility of the flame retardant foam may be reduced.
[0079] The flame retardant that can be contained in the resin composition may be subjected to a surface treatment. As such a surface treatment, any appropriate surface treatment can be adopted as long as it does not impair the effects of the present invention. Examples of such surface treatments include silane coupling treatment and stearic acid treatment.
[0080] The resin composition may contain any other appropriate components as long as the effects of the present invention are not impaired. Such other components may be one type only, or two or more types. Examples of such other components include rubber, resins other than the polymers blended as the resin material, softeners, aliphatic compounds, antiaging agents, antioxidants, light stabilizers, weathering agents, UV absorbers, dispersants, plasticizers, carbon, antistatic agents, surfactants, crosslinking agents, thickeners, rust inhibitors, silicone compounds, tension modifiers, shrinkage inhibitors, flow modifiers, gelling agents, curing agents, fillers, reinforcing agents, foaming agents, foam nucleating agents, colorants (pigments, dyes, etc.), pH adjusters, solvents (organic solvents), thermal polymerization initiators, photopolymerization initiators, lubricants, crystal nucleating agents, crystallization accelerators, vulcanizing agents, surface treatment agents, and dispersion aids.
[0081] <1-2. Formation of flame-retardant foam> The flame-retardant foam of the present invention is typically obtained by foaming a resin composition. As the foaming method (cell formation method), a method usually used in foam molding, such as a physical method or a chemical method, can be adopted. That is, the flame-retardant foam of the present invention may typically be a foam formed by foaming using a physical method (physical foam), or a foam formed by foaming using a chemical method (chemical foam). The physical method is generally a method in which a gas component such as air or nitrogen is dispersed in a polymer solution and bubbles are formed by mechanical mixing (mechanical foam). The chemical method is generally a method in which cells are formed by gas generated by thermal decomposition of a foaming agent added to a polymer base, to obtain a foam.
[0082] The resin composition to be subjected to foam molding may be prepared, for example, by mixing the components using any appropriate melt kneading device, such as an open-type mixing roll, a non-open-type Banbury mixer, a single-screw extruder, a twin-screw extruder, a continuous kneader, or a pressure kneader.
[0083] <Embodiment 1 for forming the flame-retardant foam of the present invention> One embodiment 1 of forming the flame-retardant foam of the present invention is, for example, a form in which a flame-retardant foam is formed through a step (step A) of mechanically foaming an emulsion resin composition (emulsion containing a resin material (polymer) etc.). Examples of foaming devices include high-speed shear type devices, vibration type devices, and pressurized gas discharge type devices. Among these foaming devices, high-speed shear type devices are preferred from the viewpoints of miniaturizing the bubble diameter and producing a large volume. One embodiment 1 of forming the flame-retardant foam of the present invention is applicable to formation from any resin composition.
[0084] From the viewpoint of film-forming properties, the solids concentration of the emulsion is preferably high. The solids concentration of the emulsion is preferably 30% by weight or more, more preferably 40% by weight or more, and even more preferably 50% by weight or more.
[0085] The bubbles generated by mechanical stirring are gases that have been taken into the emulsion. Any suitable gas may be used as the gas as long as it is inert to the emulsion and does not impair the effects of the present invention. Examples of such gases include air, nitrogen, and carbon dioxide.
[0086] The flame-retardant foam of the present invention can be obtained by applying the foamed emulsion resin composition (bubble-containing emulsion resin composition) onto a substrate and drying it (Step B). Examples of the substrate include a release-treated plastic film (such as a release-treated polyethylene terephthalate film), a plastic film (such as a polyethylene terephthalate film), and the like.
[0087] In step B, any appropriate method may be adopted as the coating method and drying method as long as the effects of the present invention are not impaired. Step B preferably includes a preliminary drying step B1 in which the bubble-containing emulsion resin composition applied to the substrate is dried at 50° C. or higher and lower than 125° C., and a main drying step B2 in which the composition is further dried at 125° C. or higher and 200° C. or lower.
[0088] By providing the preliminary drying step B1 and the main drying step B2, it is possible to prevent the coalescence of bubbles and the bursting of bubbles due to a sudden rise in temperature. In particular, in a foamed sheet having a small thickness, the coalescence and bursting of bubbles due to a sudden rise in temperature is likely to occur, so providing the preliminary drying step B1 is very significant. The temperature in the preliminary drying step B1 is preferably 50°C to 100°C. The time for the preliminary drying step B1 is preferably 0.5 minutes to 30 minutes, more preferably 1 minute to 15 minutes. The temperature in the main drying step B2 is preferably 130°C to 180°C or less, more preferably 130°C to 160°C. The time for the main drying step B2 is preferably 0.5 minutes to 30 minutes, more preferably 1 minute to 15 minutes.
[0089] <Embodiment 2 for forming the flame-retardant foam of the present invention> In one embodiment 2 of the present invention, the flame-retardant foam is formed by foaming the resin composition with a foaming agent. As the foaming agent, any foaming agent commonly used in foam molding can be used, and from the viewpoints of environmental protection and low pollution to the foamed object, it is preferable to use a high-pressure inert gas.
[0090] As the inert gas, any suitable inert gas may be adopted as long as it is inert to the resin composition and can be impregnated. Examples of such inert gas include carbon dioxide, nitrogen gas, and air. These gases may be used in combination. Among these, carbon dioxide is preferred from the viewpoint of a large amount of impregnation into the resin material (polymer) and a fast impregnation speed.
[0091] The inert gas is preferably in a supercritical state. That is, it is particularly preferable to use carbon dioxide in a supercritical state. In a supercritical state, the solubility of the inert gas in the resin composition is increased, making it possible to mix the inert gas at a high concentration, and the inert gas becomes highly concentrated when the pressure is suddenly lowered, so that more bubble nuclei are generated, and the density of the bubbles formed by the growth of the bubble nuclei is larger than in other states even if the porosity is the same, so that fine bubbles can be obtained. The critical temperature of carbon dioxide is 31°C, and the critical pressure is 7.4 MPa.
[0092] Examples of the method for forming a foam by impregnating a resin composition with a high-pressure inert gas include a gas impregnation step in which an inert gas is impregnated under high pressure into a resin composition containing a resin material (polymer), a depressurization step in which the pressure is reduced after the gas impregnation step to foam the resin material (polymer), and a heating step in which bubbles are grown by heating as necessary. In this case, a previously molded unfoamed molded body may be impregnated with an inert gas, or a molten resin composition may be impregnated with an inert gas under pressure and then molded during depressurization. These steps may be performed by either a batch method or a continuous method. That is, the resin composition may be molded into an appropriate shape such as a sheet to form an unfoamed resin molded body, and then the unfoamed resin molded body is impregnated with a high-pressure gas and foamed by releasing the pressure, or the resin composition may be kneaded with a high-pressure gas under pressure, and molded and foamed at the same time by releasing the pressure.
[0093] An example of producing a foam by the batch method is shown below. For example, a resin sheet for foam molding is produced by extruding a resin composition using an extruder such as a single screw extruder or a twin screw extruder. Alternatively, the resin composition is uniformly kneaded using a kneader equipped with blades such as a roller, a cam, a kneader, or a Banbury type, and pressed to a predetermined thickness using a hot plate press or the like to produce an unfoamed resin molded body. The unfoamed resin molded body thus obtained is placed in a high-pressure container, and high-pressure inert gas (such as carbon dioxide in a supercritical state) is injected to impregnate the unfoamed resin molded body with the inert gas. When the inert gas is sufficiently impregnated, the pressure is released (usually to atmospheric pressure), and bubble nuclei are generated in the resin. The bubble nuclei may be allowed to grow at room temperature as they are, or may be allowed to grow by heating in some cases. As a heating method, known or commonly used methods such as a water bath, an oil bath, a heated roll, a hot air oven, far infrared rays, near infrared rays, and microwaves can be used. After the bubbles are grown in this manner, the foam can be obtained by rapidly cooling the foam with cold water or the like to fix the shape. The unfoamed resin molded product to be foamed is not limited to a sheet-like product, and various shapes can be used depending on the application. The unfoamed resin molded product to be foamed can be produced by other molding methods such as extrusion molding, press molding, and injection molding.
[0094] An example of producing a foam by a continuous method is shown below. For example, a resin composition is kneaded using an extruder such as a single-screw extruder or a twin-screw extruder while injecting (introducing) a high-pressure gas (particularly an inert gas, or further carbon dioxide) to sufficiently impregnate the resin composition with the high-pressure gas in a kneading impregnation step, and the resin composition is extruded through a die or the like provided at the tip of the extruder to release the pressure (usually to atmospheric pressure), and foaming and foaming are simultaneously performed in a molding decompression step to form the foam. In addition, when foaming in a continuous method, a heating step for growing bubbles by heating may be provided as necessary. After the bubbles are grown in this way, the shape may be fixed by rapidly cooling with cold water or the like as necessary. The high-pressure gas may be introduced continuously or discontinuously. In addition, in the kneading impregnation step and the molding decompression step, for example, an extruder or an injection molding machine may be used. In addition, as a method of heating when growing bubble nuclei, any appropriate method such as a water bath, an oil bath, a heat roll, a hot air oven, far infrared rays, near infrared rays, and microwaves may be used. The foam may have any suitable shape, such as a sheet, a prismatic shape, a cylindrical shape, or an irregular shape.
[0095] The amount of gas mixed when foam molding the resin composition is preferably 2% by weight to 10% by weight, more preferably 2.5% by weight to 8% by weight, and even more preferably 3% by weight to 6% by weight, based on the total amount of the resin composition, in order to obtain a highly foamed product.
[0096] The pressure when the resin composition is impregnated with the inert gas can be appropriately selected in consideration of operability and the like. For example, such a pressure is preferably 6 MPa or more (for example, 6 MPa to 100 MPa), and more preferably 8 MPa or more (for example, 8 MPa to 50 MPa). In addition, the pressure when carbon dioxide in a supercritical state is used is preferably 7.4 MPa or more from the viewpoint of maintaining the supercritical state of carbon dioxide. If the pressure is lower than 6 MPa, the bubble growth during foaming is remarkable, and the bubble diameter becomes too large, so that a preferable average cell diameter (average bubble diameter) may not be obtained. This is because, when the pressure is low, the amount of gas impregnated is relatively small compared to that at high pressure, and the bubble nucleation rate decreases and the number of bubble nuclei formed decreases, so that the amount of gas per bubble increases conversely and the bubble diameter becomes extremely large. In addition, in a pressure range lower than 6 MPa, the bubble diameter and bubble density change significantly even with a small change in the impregnation pressure, so that it is easy to make it difficult to control the bubble diameter and bubble density.
[0097] The temperature in the gas impregnation step varies depending on the type of inert gas used and the type of components in the resin composition, and can be selected from a wide range. In consideration of operability, the temperature is preferably 10°C to 350°C. The impregnation temperature when impregnating an inert gas into an unfoamed molded body is preferably 10°C to 250°C, more preferably 40°C to 230°C, in the batch process. In addition, the impregnation temperature when extruding a molten polymer impregnated with a gas to simultaneously perform foaming and molding is preferably 60°C to 350°C in the continuous process. When carbon dioxide is used as the inert gas, the temperature during impregnation is preferably 32°C or higher, more preferably 40°C or higher, in order to maintain a supercritical state.
[0098] In the depressurizing step, the depressurizing speed is preferably 5 MPa / sec to 300 MPa / sec in order to obtain uniform fine bubbles.
[0099] The heating temperature in the heating step is preferably 40°C to 250°C, and more preferably 60°C to 250°C.
[0100] 2. Foam materials The foam material of the present invention has the flame-retardant foam of the present invention described above as a flame-retardant foam layer, and has a pressure-sensitive adhesive layer on at least one side of the flame-retardant foam layer.
[0101] The thickness of the flame-retardant foamed layer of the foamed material of the present invention is preferably 30 μm to 5000 μm, more preferably 35 μm to 4000 μm, further preferably 40 μm to 3000 μm, and particularly preferably 45 μm to 2500 μm. When the thickness of the flame-retardant foamed layer is within the above range, the flame-retardant foamed layer can easily conform to even a small clearance. Furthermore, when the thickness of the flame-retardant foamed layer is within the above range, bubbles can be uniformly contained, and excellent impact absorption properties can be exhibited.
[0102] The thickness of the pressure-sensitive adhesive layer is preferably 5 μm to 300 μm, more preferably 6 μm to 200 μm, further preferably 7 μm to 100 μm, and particularly preferably 8 μm to 50 μm. When the thickness of the pressure-sensitive adhesive layer is within the above range, the foam material of the present invention can exhibit excellent impact absorption properties.
[0103] The adhesive layer may be a layer made of any suitable adhesive. Examples of the adhesive constituting the adhesive layer include rubber-based adhesives (synthetic rubber-based adhesives, natural rubber-based adhesives, etc.), urethane-based adhesives, acrylic urethane-based adhesives, acrylic-based adhesives, silicone-based adhesives, polyester-based adhesives, polyamide-based adhesives, epoxy-based adhesives, vinyl alkyl ether-based adhesives, fluorine-based adhesives, and rubber-based adhesives. The adhesive constituting the adhesive layer is preferably at least one selected from acrylic-based adhesives, silicone-based adhesives, and rubber-based adhesives. Such adhesives may be of only one type or of two or more types. The adhesive layer may be of one layer or of two or more layers.
[0104] When classified according to the adhesive form, examples of the adhesive include emulsion type adhesives, solvent type adhesives, ultraviolet cross-linking type (UV cross-linking type) adhesives, electron beam cross-linking type (EB cross-linking type) adhesives, hot melt type adhesives, etc. Such adhesives may be of only one type or of two or more types.
[0105] The water vapor permeability of the adhesive layer is preferably 50 (g / (m 2 24 hours) or less, and more preferably 30 (g / (m 2 24 hours) or less, and more preferably 20 (g / (m 2 24 hours) or less, and particularly preferably 10 (g / (m 2 When the water vapor permeability of the pressure-sensitive adhesive layer is within the above range, the foam sheet of the present invention is not affected by moisture and can stabilize the impact absorption properties.
[0106] The adhesive constituting the adhesive layer may contain any appropriate other component within a range that does not impair the effects of the present invention.
[0107] Examples of the other components include other polymer components, softeners, antiaging agents, curing agents, plasticizers, fillers, antioxidants, thermal polymerization initiators, photopolymerization initiators, ultraviolet absorbers, light stabilizers, colorants (pigments, dyes, etc.), solvents (organic solvents), surfactants (e.g., ionic surfactants, silicone-based surfactants, fluorine-based surfactants, etc.), crosslinking agents (e.g., polyisocyanate-based crosslinking agents, silicone-based crosslinking agents, epoxy-based crosslinking agents, alkyl etherified melamine-based crosslinking agents, etc.), etc. The thermal polymerization initiator and the photopolymerization initiator can be included in the material for forming the polymer component.
[0108] The foamed material of the present invention can be produced by any appropriate method, such as a method of producing the foamed material of the present invention by laminating a flame-retardant foam layer and a pressure-sensitive adhesive layer, or a method of producing the foamed material of the present invention by laminating a material for forming a pressure-sensitive adhesive layer and a flame-retardant foam layer and then forming a pressure-sensitive adhesive layer by a curing reaction or the like. EXAMPLES
[0109] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. The test and evaluation methods in the examples are as follows. The term "parts" means "parts by weight" unless otherwise specified, and the term "%" means "% by weight" unless otherwise specified.
[0110] <Method of measuring apparent density> The density (apparent density) of the flame-retardant foam was calculated as follows. The resin foam structures obtained in the examples and comparative examples were punched out to a size of 20 mm x 20 mm to prepare test pieces, and the dimensions of the test pieces were measured with a vernier caliper. Next, the weight of the test pieces was measured with an electronic balance. Then, the density was calculated according to the following formula. Apparent density (g / cm 3 ) = weight of test piece / volume of test piece
[0111] <Method of measuring 50% compression load> The measurement was performed according to the method for measuring the compression hardness of foams described in JIS K 6767. Specifically, the resin foam structures obtained in the examples and comparative examples were cut into test pieces of 30 mm × 30 mm size, and the stress (N) when compressed to a compression rate of 50% at a compression speed of 10 mm / min was measured per unit area (1 cm 2 ) converted to 50% compression load (N / cm 2 ) was decided.
[0112] <Method of measuring breaking elongation in tensile test> The measurement was performed according to the method for measuring tensile elongation of foams described in JIS K 6767.
[0113] <Method of measuring the average bubble size (average cell size) and coefficient of variation of bubble size (cell size)> A digital microscope (product name "VHX-500", manufactured by Keyence Corporation) was used as a measuring instrument to capture enlarged images of the bubbles in the resin foam structures obtained in the Examples and Comparative Examples, and the average bubble diameter (average cell diameter) (μm) was determined by analyzing the images using the analysis software of the measuring instrument. The number of bubbles in the captured enlarged image was about 400. In addition, the standard deviation was calculated from all the cell diameter data, and the coefficient of variation was calculated using the following formula. Coefficient of variation = standard deviation / average bubble size (average cell size)
[0114] <Method of measuring bubble rate (cell rate)> Measurements were performed in an environment with a temperature of 23°C and a humidity of 50%. The resin foam structures obtained in the Examples and Comparative Examples were punched out using a punching blade of 100 mm x 100 mm, and the dimensions of the punched samples were measured. In addition, the thickness was measured using a 1 / 100 dial gauge with a measuring terminal diameter (φ) of 20 mm. From these values, the volumes of the resin foam structures obtained in the Examples and Comparative Examples were calculated. Next, the weights of the resin foam structures obtained in the Examples and Comparative Examples were measured using a top-pan balance with a minimum scale of 0.01 g or more. From these values, the foam ratios (cell ratios) of the resin foam structures obtained in the Examples and Comparative Examples were calculated.
[0115] <Method of measuring bubble wall (cell wall) thickness> A digital microscope (product name "VHX-500", manufactured by Keyence Corporation) was used as a measuring instrument to capture enlarged images of the bubbles in the resin foam structures obtained in the Examples and Comparative Examples, and the thickness (μm) of the bubble walls (cell walls) was determined by analyzing the images using the analysis software of the measuring instrument. The number of bubbles in the captured enlarged images was about 400.
[0116] <Method for measuring residue of flame-retardant foam at 650℃> 5 mg of the resin foam structures obtained in the Examples and Comparative Examples were placed in a platinum container, and the temperature was increased at a heating rate of 20°C / min in the measurement range from 25°C to 680°C under a nitrogen gas atmosphere, and the residue at 650°C was measured using TG / DTA6200 (manufactured by SII Nano Technology Co., Ltd.).
[0117] <How to measure horizontal burning distance> Measurements were conducted in accordance with the flame retardancy test method for foams described in UL 94. The smaller the horizontal burning distance, the better the flame retardancy tends to be.
[0118] <Method for measuring stress distribution> FIG. 1 is a schematic cross-sectional view of a stress relaxation tester 1000 used to measure the degree of stress dispersion. As shown in FIG. 1, a polycarbonate plate (200 mm×300 mm×thickness 1 mm) 200 was placed on an iron support 100, and a stress measurement film 300 (product name "Prescale" (two sheets, for low pressure (4LW), Fujifilm Corporation, a sheet with a surface that changes color when pressure is applied, 50 mm×50 mm×thickness 0.16 mm) was placed on top of the polycarbonate plate 200. Next, on the stress measurement film 300, examples and comparative examples of the measurement target were The resin foam structure (150 mm x 200 mm x 0.5 mm thick) 400 obtained in the above step was placed, double-sided adhesive tape (No. 5603, manufactured by Nitto Denko, thickness 0.03 mm) 500 was attached on top of it, a 0.3 mm thick spacer 600 was placed, and an ABS plate (200 mm x 300 mm x thickness 3 mm) 700 was placed on top. An iron ball (φ25 mm) 800 was placed in the center on top of it, and a load of 100 N was applied for 1 minute. Thereafter, the color change of the stress measurement film 300 was observed, and those in which the color did not spread from the center of the stress measurement film 300 but was dot-like were rated C, those in which the color spread 25 mm from the center of the stress measurement film 300 were rated B, and those in which the color spread widely 50 mm from the center of the stress measurement film 300 to the edge were rated A.
[0119] Example 1 Polypropylene [melt flow rate (MFR) (230°C): 0.40g / 10min]: 32.5 parts by weight, polypropylene [melt flow rate (MFR) (230°C): 1.1g / 10min]: 32.5 parts by weight, polyolefin elastomer [trade name "Thermorun 5850N", manufactured by Mitsubishi Chemical]: 35 parts by weight, magnesium hydroxide: 120 parts by weight (trade name "MGZ-1", manufactured by Sakai Chemical Industry Co., Ltd.), carbon (trade name "Asahi #35", manufactured by Asahi Carbon Co., Ltd.): 10 parts by weight, and stearic acid monoglyceride: 1 part by weight were kneaded at a temperature of 200°C in a twin-screw kneader manufactured by Japan Steel Works (JSW), extruded into a strand shape, cooled with water, and molded into pellets. The pellets were put into a single-screw extruder manufactured by Japan Steel Works, and carbon dioxide gas was injected at a pressure of 13 (12 after injection) MPa in an atmosphere of 220°C. Carbon dioxide gas was injected at a ratio of 3 parts by weight per 100 parts by weight of the resin. After being fully saturated with carbon dioxide gas, the resin was cooled to a temperature suitable for foaming and extruded through a die to obtain a sheet-like resin foam structure (1) having a thickness of 2.2 mm. In this resin foam structure (1), the apparent density is 0.07 g / cm 3 , 50% compression load is 4.0N / cm 2 , and the breaking elongation was 89%. The results are shown in Table 1.
[0120] Example 2 Polypropylene [melt flow rate (MFR) (230°C): 0.40g / 10min]: 32.5 parts by weight, polypropylene [melt flow rate (MFR) (230°C): 1.1g / 10min]: 32.5 parts by weight, polyolefin elastomer [trade name "Milastomer 8030N", manufactured by Mitsui Chemicals]: 35 parts by weight, magnesium hydroxide: 120 parts by weight (trade name "KISUMA 5P, manufactured by Kyowa Chemical Industry Co., Ltd.), carbon (trade name "Asahi #35", manufactured by Asahi Carbon Co., Ltd.): 10 parts by weight, and stearic acid monoglyceride: 1 part by weight were kneaded at a temperature of 200°C in a twin-screw kneader manufactured by Japan Steel Works (JSW), extruded into a strand shape, cooled with water, and molded into pellets. The pellets were put into a single-screw extruder manufactured by Japan Steel Works, and carbon dioxide gas was injected at a pressure of 13 (12 after injection) MPa in an atmosphere of 220°C. Carbon dioxide gas was injected at a ratio of 3 parts by weight per 100 parts by weight of the resin. After being fully saturated with carbon dioxide gas, the resin was cooled to a temperature suitable for foaming and extruded from a die to obtain a sheet-like resin foam structure (2) having a thickness of 2.2 mm. In this resin foam structure (2), the apparent density is 0.07 g / cm 3 , 50% compression load is 3.5N / cm 2 , and the breaking elongation was 77%. The results are shown in Table 1.
[0121] Example 3 Polypropylene [melt flow rate (MFR) (230°C): 0.40g / 10min]: 19 parts by weight, polypropylene [melt flow rate (MFR) (230°C): 1.1g / 10min]: 19 parts by weight, polyolefin elastomer [trade name "Milastomer 8030N", manufactured by Mitsui Chemicals]: 67 parts by weight, magnesium hydroxide: 80 parts by weight (trade name "KISUMA 5P", manufactured by Kyowa Chemical Industry Co., Ltd.), carbon (trade name "Asahi #35", manufactured by Asahi Carbon Co., Ltd.): 10 parts by weight, and stearic acid monoglyceride: 1 part by weight were kneaded at a temperature of 200°C in a twin-screw kneader manufactured by Japan Steel Works (JSW), extruded into a strand shape, cooled with water, and molded into pellets. The pellets were put into a single-screw extruder manufactured by Japan Steel Works, and carbon dioxide gas was injected at a pressure of 13 (12 after injection) MPa in an atmosphere of 220°C. Carbon dioxide gas was injected at a ratio of 3 parts by weight per 100 parts by weight of the resin. After being fully saturated with carbon dioxide gas, the resin was cooled to a temperature suitable for foaming and extruded through a die to obtain a sheet-like resin foam structure (3) having a thickness of 1.8 mm. In this resin foam structure (3), the apparent density is 0.07 g / cm 3 , 50% compression load is 1.7N / cm 2 The elongation at break was 90%. The results are shown in Table 1.
[0122] Example 4 Polypropylene [melt flow rate (MFR) (230°C): 0.40g / 10min]: 16.5 parts by weight, polypropylene [melt flow rate (MFR) (230°C): 1.1g / 10min]: 16.5 parts by weight, polyolefin elastomer [trade name "Milastomer 8030N", manufactured by Mitsui Chemicals]: 67 parts by weight, magnesium hydroxide: 60 parts by weight (trade name "KISUMA 5P", manufactured by Kyowa Chemical Industry Co., Ltd.), carbon (trade name "Asahi #35", manufactured by Asahi Carbon Co., Ltd.): 10 parts by weight, and stearic acid monoglyceride: 1 part by weight were kneaded at a temperature of 200°C in a twin-screw kneader manufactured by Japan Steel Works (JSW), extruded into a strand shape, cooled with water, and molded into pellets. The pellets were put into a single-screw extruder manufactured by Japan Steel Works, and carbon dioxide gas was injected at a pressure of 13 (12 after injection) MPa in an atmosphere of 220°C. Carbon dioxide gas was injected at a ratio of 3 parts by weight per 100 parts by weight of the resin. After being fully saturated with carbon dioxide gas, the resin was cooled to a temperature suitable for foaming and extruded from a die to obtain a sheet-like resin foam structure (4) having a thickness of 1.8 mm. In this resin foam structure (4), the apparent density is 0.085 g / cm 3 , 50% compression load is 2.1N / cm 2 The elongation at break was 85%. The results are shown in Table 1.
[0123] Example 5 Polypropylene [melt flow rate (MFR) (230°C): 0.40g / 10min]: 20.5 parts by weight, polypropylene [melt flow rate (MFR) (230°C): 1.1g / 10min]: 20.5 parts by weight, polyolefin elastomer [trade name "Milastomer 8030N", manufactured by Mitsui Chemicals]: 59 parts by weight, magnesium hydroxide: 60 parts by weight (trade name "KISUMA 5P", manufactured by Kyowa Chemical Industry Co., Ltd.), carbon (trade name "Asahi #35", manufactured by Asahi Carbon Co., Ltd.): 100 parts by weight, and stearic acid monoglyceride: 1 part by weight were kneaded at a temperature of 200°C in a twin-screw kneader manufactured by Japan Steel Works (JSW), extruded into a strand shape, cooled with water, and molded into pellets. The pellets were put into a single-screw extruder manufactured by Japan Steel Works, and carbon dioxide gas was injected at a pressure of 13 (12 after injection) MPa in an atmosphere of 220°C. Carbon dioxide gas was injected at a ratio of 3 parts by weight per 100 parts by weight of the resin. After being fully saturated with carbon dioxide gas, the resin was cooled to a temperature suitable for foaming and extruded through a die to obtain a sheet-like resin foam structure (5) having a thickness of 1.8 mm. In this resin foam structure (5), the apparent density is 0.085 g / cm 3 , 50% compression load is 2.9N / cm 2 The elongation at break was 80%. The results are shown in Table 1.
[0124] Comparative Example 1 Polypropylene [melt flow rate (MFR) (230°C): 0.40g / 10min]: 16.5 parts by weight, polypropylene [melt flow rate (MFR) (230°C): 1.1g / 10min]: 16.5 parts by weight, polyolefin elastomer [trade name "Thermorun 5850N", manufactured by Mitsubishi Chemical]: 67 parts by weight, magnesium hydroxide: 40 parts by weight (trade name "KISUMA 5P", manufactured by Kyowa Chemical Industry Co., Ltd.), carbon (trade name "Asahi #35", manufactured by Asahi Carbon Co., Ltd.): 10 parts by weight, and stearic acid monoglyceride: 1 part by weight were kneaded at a temperature of 200°C in a twin-screw kneader manufactured by Japan Steel Works (JSW), extruded into a strand shape, cooled with water, and molded into pellets. The pellets were put into a single-screw extruder manufactured by Japan Steel Works, and carbon dioxide gas was injected at a pressure of 13 (12 after injection) MPa in an atmosphere of 220°C. Carbon dioxide gas was injected at a ratio of 3 parts by weight per 100 parts by weight of the resin. After being fully saturated with carbon dioxide gas, the mixture was cooled to a temperature suitable for foaming and extruded from a die to obtain a sheet-like resin foam structure (C1) having a thickness of 1.8 mm. In this resin foam structure (C1), the apparent density is 0.065 g / cm 3 , 50% compression load is 1.8N / cm 2 The elongation at break was 140%. The results are shown in Table 1.
[0125] Comparative Example 2 The foam containing polyurethane as a main component was used as a resin foam structure (C2). In this resin foam structure (C2), the apparent density is 0.40 g / cm 3 , 50% compression load is 12N / cm 2 The elongation at break was 130%. The results are shown in Table 1.
[0126] Comparative Example 3 Polypropylene [density: 0.9g / cm 3, melt flow rate (MFR) (230 ° C): 4g / 10min]: 50 parts by weight, olefin-based elastomer [trade name "Milastomer 8030N", manufactured by Mitsui Chemicals]: 50 parts by weight, carbon black manufactured by the oil furnace method: 10 parts by weight, polyhedral composite metal hydroxide (average particle size 0.7 μm) represented by the formula MgO·NiO·H2O: 100 parts by weight were kneaded at a temperature of 180 ° C by a Labo Plastomill (manufactured by Toyo Seiki Seisakusho) equipped with roller-type blades, and then molded into a sheet shape of 0.5 mm in thickness and φ80 mm using a hot plate press heated to 180 ° C. This sheet was placed in a pressure-resistant container and impregnated with carbon dioxide by holding it for 10 minutes under a pressure of 15 MPa in an atmosphere of 150 ° C. Then, the pressure was suddenly reduced to obtain a resin foam structure (C3). In this resin foam structure (C3), the apparent density is 0.033 g / cm 3 , 50% compression load is 2.49N / cm 2 The elongation at break was 140%. The results are shown in Table 1.
[0127] Comparative Example 4 An acrylic emulsion solution (solid content 55%, ethyl acrylate-butyl acrylate-acrylonitrile copolymer (weight ratio of monomers used: 45:48:7)): 100 parts by weight, a fatty acid ammonium surfactant (aqueous dispersion of ammonium stearate, solid content 33%) (surfactant A): 2 parts by weight, a carboxybetaine type amphoteric surfactant ("Amogen CB-H", Daiichi Kogyo Seiyaku Co., Ltd.) (surfactant B): 2 parts by weight, an oxazoline crosslinking agent ("Epocross WS-500", Nippon Shokubai Co., Ltd., solid content 39%): 4 parts by weight, and a pigment (carbon black) ("NAF-5091", Dainichiseika Color & Chemicals Co., Ltd.): 1 part by weight were stirred and mixed in a disper ("Robomix", Primix Corporation) to generate foam. This foaming composition was applied onto a release-treated PET (polyethylene terephthalate) film (thickness: 38 μm, product name "MRF#38", manufactured by Mitsubishi Plastics, Inc.), and dried at 70°C for 4.5 minutes and at 140°C for 4.5 minutes to obtain a resin foam structure (C4) (thickness: 0.20 mm). In this resin foam structure (C4), the apparent density is 0.70 g / cm 3 , 50% compression load is 7.2N / cm 2 The elongation at break was 100%. The results are shown in Table 1.
[0128] Comparative Example 5 Acrylic emulsion solution (solid content 55%, ethyl acrylate-butyl acrylate-acrylonitrile copolymer (weight ratio of monomers used: 45:48:7)): 100 parts by weight, fatty acid ammonium surfactant (aqueous dispersion of ammonium stearate, solid content 33%) (surfactant A): 1.6 parts by weight, carboxybetaine type amphoteric surfactant ("Amogen CB-H", Daiichi Kogyo Seiyaku Co., Ltd.) (surfactant B): 1.6 parts by weight, oxazoline crosslinking agent ("Epocross WS-500", Nippon Shokubai Co., Ltd., solid content 39%): 4 parts by weight, pigment (carbon black) ("NAF-5091", Dainichiseika Color & Chemicals Co., Ltd.): 2 parts by weight, polyacrylic acid thickener (ethyl acrylate-acrylic acid copolymer (content ratio of monomers used: 20% by weight of acrylic acid, solid content 28.7%): 0.8 parts by weight, surface-treated silica particles ("Nipsil E150J, manufactured by Tosoh Silica Corporation): 25 parts by weight were stirred and mixed in a Disper (Robomix, manufactured by Primix Corporation) to generate foam. This foaming composition was applied to a release-treated PET (polyethylene terephthalate) film (thickness: 38 μm, product name "MRF♯38", manufactured by Mitsubishi Plastics, Inc.), and dried at 70°C for 4.5 minutes and at 140°C for 4.5 minutes to obtain a resin foam structure (C5) (thickness: 0.20 mm). In this resin foam structure (C5), the apparent density is 0.30 g / cm 3 , 50% compression load is 11N / cm 2 The elongation at break was 80%. The results are shown in Table 1.
[0129] [Table 1]
[0130] [Production Example 1] In a reaction vessel equipped with a stirrer, a thermometer, a nitrogen gas inlet tube, a reflux condenser, and a dropping funnel, 60 parts of butyl acrylate (BA), 40 parts of 2-ethylhexyl acrylate (2EHA), 5 parts of acrylic acid (AA) as monomer components, and 135 parts of toluene as a polymerization solvent were charged, and the mixture was stirred for 2 hours while introducing nitrogen gas. After removing oxygen from the polymerization system in this way, 0.1 parts of azobisisobutyronitrile (AIBN) as a polymerization initiator was added, and solution polymerization was carried out at 60°C for 6 hours to obtain a toluene solution of an acrylic polymer. The Mw of this acrylic polymer was 40×10 4 It was. To 100 parts of the acrylic polymer contained in the toluene solution, 30 parts of a polymerized rosin ester (trade name "PENSEL D-125", softening point 120-130°C, manufactured by Arakawa Chemical Industries Co., Ltd.) as a tackifier resin and 2 parts of an isocyanate crosslinking agent (trade name "CORONATE L", manufactured by Tosoh Corporation, solid content 75%) were added to prepare an acrylic adhesive composition. This acrylic adhesive composition was applied to a release-treated PET (polyethylene terephthalate) film (thickness: 38 μm, trade name "MRF♯38", manufactured by Mitsubishi Plastics, Inc.) and dried at 120°C for 5 minutes to obtain an adhesive layer (1) having a thickness of 30 μm.
[0131] Example 6 The pressure-sensitive adhesive layer (1) obtained in Production Example 1 was bonded to one side of the resin foam structure (1) obtained in Example 1 to obtain a foam material (1) having a two-layer structure of resin foam structure (1) / pressure-sensitive adhesive layer (1).
[0132] Example 7 The pressure-sensitive adhesive layers (1) obtained in Production Example 1 were bonded to both sides of the resin foam structure (1) obtained in Example 1 to obtain a foam material (2) having a three-layer structure of pressure-sensitive adhesive layer (1) / resin foam structure (1) / pressure-sensitive adhesive layer (1). [Industrial Applicability]
[0133] The flame-retardant foam of the present invention can be suitably used, for example, as a flame-retardant foam for electronic devices. [Explanation of symbols]
[0134] Stress Relaxation Tester 1000 Iron support 100 Polycarbonate sheet 200 Stress measurement film 300 Resin foam structure 400 Double-sided adhesive tape 500 Spacer 600 ABS board 700 Iron ball 800
Claims
1. Apparent density is 0.02 g / cm 3 ~0.40g / cm 3 and 50% compression load is 0.5N / cm 2 ~8.0N / cm 2 and The breaking elongation in a tensile test is 120% or less, The coefficient of variation of the bubble diameter is 0.5 or less. Flame retardant foam.
2. The flame-retardant foam according to claim 1, having an average cell diameter of 10 μm to 200 μm.
3. The flame-retardant foam according to claim 1 or 2, having a foaming rate of 30% or more.
4. 4. The flame retardant foam of claim 1, wherein the cell wall has a thickness of 0.1 μm to 10 μm.
5. 5. The flame retardant foam of claim 1 comprising a flame retardant.
6. 6. The flame retardant foam of claim 5, wherein the flame retardant comprises a non-halogen, non-antimony flame retardant.
7. The bulk density of the flame retardant is 0.8 g / cm 3 7. The flame retardant foam of claim 5, wherein:
8. 8. The flame-retardant foam according to claim 1, having a residue at 650° C. of 20% by weight or more.
9. The flame-retardant foam according to claim 1 , wherein the resin constituting the flame-retardant foam is a polyolefin-based resin.
10. The flame-retardant foam according to claim 9, wherein the polyolefin-based resin is a mixture of a polypropylene other than a polyolefin-based elastomer and a polyolefin-based elastomer.
11. A foam member, comprising the flame-retardant foam according to any one of claims 1 to 10 as a flame-retardant foam layer, and having a pressure-sensitive adhesive layer on at least one side of the flame-retardant foam layer.
Citation Information
Patent Citations
Thermoplastic foam article and its preparation
JP1994322168A
Flame-retardant resin foam
JP2003165860A
Halogen-free heat-insulating flame-retardant sponge
JP2007204621A
Resin composition for polyolefinic resin foam, polyolefinic resin foam, and foaming seal material
JP2013049830A
Flame-retardant resin foams and flame-retardant foamed members
WO2010106912A1