Sheet for sealing optical semiconductor elements and method for producing optical semiconductor device

The sealing sheet with a radiation-non-curable adhesive layer and radiation-curable resin layer addresses the issues of adhesion and damage in optical semiconductor devices, facilitating easy positional correction and reducing manufacturing costs for large-screen displays.

JP7572264B2Active Publication Date: 2024-10-23NITTO DENKO CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021028574
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-25
Publication Date
2024-10-23
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

The existing methods for sealing optical semiconductor devices using liquid resin face issues such as poor handling, adhesion to unintended areas, and damage during tiling due to sheet adhesion and separation, particularly affecting large-screen image display devices.

Method used

A sealing sheet for optical semiconductor elements is designed with a radiation-non-curable adhesive layer and a radiation-curable resin layer, which reduces adhesion between adjacent devices during separation and enhances handling, allowing for easy positional correction and reduced damage.

Benefits of technology

The sheet provides excellent sealing properties and adhesion to optical semiconductor elements, preventing sheet damage and adhesion during separation, enabling efficient manufacturing of large-screen displays with improved yield and reduced costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572264000002
    Figure 0007572264000002
  • Figure 0007572264000003
    Figure 0007572264000003
  • Figure 0007572264000004
    Figure 0007572264000004
Patent Text Reader

Abstract

To provide an optical semiconductor element encapsulation sheet with excellent encapsulation properties of an optical semiconductor element, being less likely to occur a loss of a sheet and adhesion of sheets of adjacent optical semiconductor devices when the adjacent optical semiconductor devices are separated from each other.SOLUTION: An optical semiconductor element encapsulation sheet 1 is a sheet for encapsulating one or more optical semiconductor elements 6 arranged on a substrate 5. The optical semiconductor element encapsulation sheet 1 comprises a base material part 2, and an encapsulation part 3 provided on one surface of the base material part 2. The encapsulation part 3 encapsulates the optical semiconductor elements 6. The encapsulation part 3 has a radiation non-curable adhesive layer 32, and a radiation curable resin layer 31 laminated on the radiation non-curable adhesive layer 32. The radiation non-curable adhesive layer 32 is positioned on a surface on the optical semiconductor element 6 side when the optical semiconductor elements 6 are encapsulated.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a sheet for encapsulating optical semiconductor elements. More specifically, the present invention relates to a sheet for encapsulating one or more optical semiconductor elements arranged on a substrate. The present invention also relates to a method for producing an optical semiconductor device. [Background technology]

[0002] For example, a backlight used in a liquid crystal display device is known to have a structure in which a plurality of LEDs are arranged on a substrate and the plurality of LEDs are sealed with a sealing resin. As a method for sealing the plurality of LEDs collectively using the sealing resin, a method is known in which liquid resin is poured into the area where the plurality of LEDs are arranged, the plurality of LEDs are buried, and then the liquid resin is cured by applying heat or ultraviolet rays (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2017-66390 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the method of using liquid resin to encapsulate optical semiconductor elements such as LEDs has problems such as poor handling, such as dripping when the liquid resin is applied and the liquid resin adhering to unintended areas.

[0005] In contrast, by using an encapsulating sheet having an encapsulating layer for encapsulating an optical semiconductor element instead of using a liquid resin, it is possible to encapsulate the optical semiconductor element easily and in a short time. Here, it is important that the encapsulating sheet has excellent encapsulation properties for the optical semiconductor element and excellent adhesion to the optical semiconductor element and the substrate having the optical semiconductor element in order to encapsulate the optical semiconductor element sufficiently.

[0006] Meanwhile, with the trend toward higher image quality such as 4K and 8K, the demand for image display devices with larger screens is growing. In addition, the use of image display devices with larger screens for signage such as advertising displays and bulletin boards outdoors and in public facilities is also progressing. However, manufacturing image display devices with larger screens causes problems such as a lower yield and an increase in manufacturing costs. In order to manufacture large-screen image display devices at lower cost, a tiling display in which multiple optical semiconductor devices such as image display devices are arranged in a tiled shape is being considered. When multiple optical semiconductor devices are arranged in a tiled shape, i.e., when tiling, if a positional deviation occurs between adjacent optical semiconductor devices or if rearrangement is required, position correction is performed.

[0007] Here, when tiling optical semiconductor devices in which an optical semiconductor element is encapsulated by an encapsulating sheet, it is necessary to once separate adjacent optical semiconductor devices in order to correct the position during tiling. However, when separating them, the encapsulating sheet of one optical semiconductor device and the encapsulating sheet of the other adjacent optical semiconductor device may adhere to each other and attract each other, causing defects such as defects in the encapsulating sheet of one optical semiconductor device or a part of the encapsulating sheet being transferred and attached to the other optical semiconductor device. Such defects are particularly likely to occur in encapsulating sheets that have excellent adhesion to optical semiconductor elements and substrates.

[0008] The present invention was devised under these circumstances, and its object is to provide a sheet for sealing optical semiconductor elements which has excellent sealing properties for optical semiconductor elements, while preventing damage to the sheet or adhesion of the sheets of adjacent optical semiconductor devices when separating the adjacent optical semiconductor devices. [Means for solving the problem]

[0009] As a result of intensive research to achieve the above object, the present inventors have found that a sheet for encapsulating optical semiconductor elements, which comprises an encapsulating part having a non-radiation-curable pressure-sensitive adhesive layer and a radiation-curable resin layer, with the non-radiation-curable pressure-sensitive adhesive layer located on the surface of the encapsulating part facing the optical semiconductor element, has excellent encapsulation properties for optical semiconductor elements, while being less susceptible to damage to the sheet or adhesion of the sheets of adjacent optical semiconductor devices when the devices are separated from each other. The present invention was completed based on these findings.

[0010] That is, the present invention provides a sheet for encapsulating one or more optical semiconductor elements disposed on a substrate, comprising: a substrate and a sealing portion provided on one surface of the substrate for sealing the optical semiconductor element; The present invention provides a sheet for encapsulating optical semiconductor elements, wherein the encapsulating portion has a non-radiation-curable pressure-sensitive adhesive layer that is located on the surface facing the optical semiconductor element when the optical semiconductor element is encapsulated, and a radiation-curable resin layer that is laminated on the non-radiation-curable pressure-sensitive adhesive layer.

[0011] As described above, the sheet for encapsulating optical semiconductor elements includes an encapsulation portion in which a non-radiation-curable pressure-sensitive adhesive layer and a radiation-curable resin layer are laminated. The encapsulation portion is an area of ​​the sheet for encapsulating an optical semiconductor element that encapsulates the optical semiconductor element. The non-radiation-curable pressure-sensitive adhesive layer is located on the surface of the encapsulation portion that faces the optical semiconductor element when encapsulating the optical semiconductor element. By having the non-radiation-curable pressure-sensitive adhesive layer located on the surface, when the sheet for encapsulating an optical semiconductor element encapsulates the optical semiconductor element, the non-radiation-curable pressure-sensitive adhesive layer has excellent adhesion to the optical semiconductor element and the substrate, and the sheet for encapsulating an optical semiconductor element has excellent encapsulation properties. After encapsulation, the radiation-curable resin layer is cured by irradiation with radiation, and the adhesion of the encapsulating sheet side surface is reduced. As a result, the adhesion between the encapsulation portions of adjacent optical semiconductor devices in a tiling state is low, and when adjacent optical semiconductor devices are separated from each other, the sheet is less likely to be damaged or the sheets of adjacent optical semiconductor devices are less likely to adhere to each other. In addition, the substrate portion serves as a support for the encapsulation portion, and the sheet for encapsulating an optical semiconductor device has excellent handleability due to the substrate portion. Furthermore, when dicing an optical semiconductor device after encapsulating an optical semiconductor element with the sheet for encapsulating an optical semiconductor element to produce the optical semiconductor device, stickiness at the diced portion can be further suppressed, making it possible to produce an optical semiconductor device with a good appearance.

[0012] The radiation curable resin layer is preferably thicker than the non-radiation curable adhesive layer. With this configuration, the low adhesion between the radiation curable resin layers in adjacent optical semiconductor devices after curing becomes dominant over the high adhesion between the non-radiation curable adhesive layers in adjacent optical semiconductor devices in a tiling state, so that the adhesion between the sealing parts is further lower, and when the adjacent optical semiconductor devices are separated from each other, the sheet is less likely to be damaged or the sheets of the adjacent optical semiconductor devices are less likely to adhere to each other. In addition, when dicing the optical semiconductor device after sealing the optical semiconductor element with the sheet for sealing the optical semiconductor element, the stickiness of the diced part can be further suppressed, and an optical semiconductor device with a good appearance can be produced.

[0013] The sealing portion may include a layer containing a colorant. With such a configuration, when the optical semiconductor device is tiled and applied to a display, it is possible to suppress color mixing of light emitted by each optical semiconductor element when the optical semiconductor device is in use, and to adjust the appearance of the display when the optical semiconductor device is not in use.

[0014] The optical semiconductor element encapsulation sheet preferably includes a layer having antiglare and / or antireflection properties. With such a configuration, when the optical semiconductor device is tiled and applied to a display, the gloss and light reflection of the display can be suppressed, and the appearance of the display can be improved.

[0015] The optical semiconductor element encapsulation sheet preferably includes a layer mainly composed of a polyester resin and / or a polyimide resin. With such a configuration, the optical semiconductor element encapsulation sheet has excellent heat resistance, and the thermal expansion of the optical semiconductor element encapsulation sheet can be suppressed in a high-temperature environment, improving dimensional stability. In addition, the sheet can be given rigidity, improving handling and retention.

[0016] The hardness of a cross section of the radiation curable resin layer after curing, measured by nanoindentation at a temperature of 23° C., is preferably 1.4 MPa or greater. By having such a configuration, the radiation curable resin layer has an appropriate hardness after curing, making it even less likely that the sheet will be damaged or that the sheets of adjacent optical semiconductor devices will adhere to each other when they are separated from each other in a tiling state.

[0017] The present invention also provides an optical semiconductor device comprising a substrate, an optical semiconductor element disposed on the substrate, and a cured product formed by curing the radiation curable resin layer of the sheet for encapsulating an optical semiconductor element, which encapsulates the optical semiconductor element. In such an optical semiconductor device, after the radiation curable resin has been cured, damage to the sheet or adhesion of the sheets of adjacent optical semiconductor devices is unlikely to occur when adjacent optical semiconductor devices are separated from each other. In addition, stickiness of the diced portion can be suppressed during dicing, making it possible to produce an optical semiconductor device with good appearance.

[0018] The optical semiconductor device may be a backlight for a liquid crystal screen. The optical semiconductor device may also be a self-luminous display device. The optical semiconductor device has a good appearance when applied to an optical semiconductor device having a display, and is therefore preferably applied as a backlight for a liquid crystal screen or a self-luminous display device.

[0019] The present invention also provides an image display device including the above-mentioned backlight and a display panel.

[0020] The present invention also provides an image display device including the above-mentioned self-luminous display device.

[0021] The present invention also provides a method for producing an optical semiconductor device, comprising a dicing step of dicing a laminate comprising a substrate, an optical semiconductor element disposed on the substrate, and a cured product obtained by curing the radiation-curable resin layer of the sheet for encapsulating an optical semiconductor element, the cured product encapsulating the optical semiconductor element, to obtain an optical semiconductor device.

[0022] When the radiation curable resin layer is irradiated with radiation and cured, curing is inhibited on the side where oxygen is present, and curing is likely to be insufficient. In contrast, according to the above-mentioned manufacturing method including the dicing step, for a laminate including a cured product of a sheet for encapsulating optical semiconductor elements, including a cured encapsulating layer obtained by curing the radiation curable resin layer by irradiation with radiation, the side end portion that is insufficiently cured in the dicing step is cut off and removed, thereby obtaining an optical semiconductor device in which an area that has been sufficiently cured and has reduced adhesion is exposed on the side. In the optical semiconductor device manufactured in this way, the adhesion of the side surface of the radiation curable resin layer after curing is sufficiently reduced, so that when adjacent optical semiconductor devices are separated from each other in a tiling state, the sheet is unlikely to be damaged or the sheets of adjacent optical semiconductor devices are unlikely to adhere to each other.

[0023] The above-mentioned manufacturing method may further include a radiation exposure step of irradiating a laminate comprising the above-mentioned substrate, an optical semiconductor element disposed on the above-mentioned substrate, and the sheet for encapsulating an optical semiconductor element that encapsulates the optical semiconductor element with radiation to cure the radiation-curable resin layer and obtain the cured product.

[0024] The manufacturing method may include a sealing step of bonding the sheet for encapsulating an optical semiconductor element to the optical semiconductor element provided on the substrate to encapsulate the optical semiconductor element with the encapsulating portion, and then carrying out the radiation irradiation step.

[0025] The manufacturing method may further include a tiling step of arranging the multiple optical semiconductor devices obtained in the dicing step so as to be in contact with each other in a planar direction. Effect of the Invention

[0026] According to the sheet for encapsulating optical semiconductor elements of the present invention, while having excellent encapsulation properties for optical semiconductor elements, when adjacent optical semiconductor devices are separated from each other, the sheet is unlikely to be damaged or the sheets of adjacent optical semiconductor devices are unlikely to adhere to each other. Therefore, when the adjacent optical semiconductor devices are displaced from each other or when rearrangement is required after tiling of the optical semiconductor devices, the position can be easily corrected without any trouble, the loss of the optical semiconductor devices can be reduced, and a display with a good appearance can be produced economically. [Brief description of the drawings]

[0027] [Figure 1] 1 is a cross-sectional view of a sheet for encapsulating an optical semiconductor element according to one embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view of an optical semiconductor device using a sheet for encapsulating an optical semiconductor element according to one embodiment of the present invention. [Diagram 3] 3 is an external view showing one embodiment of an optical semiconductor device produced by tiling the optical semiconductor device shown in FIG. 2. [Figure 4] 4A to 4C are cross-sectional views illustrating a sealing step in one embodiment of a method for manufacturing an optical semiconductor device. [Diagram 5] FIG. 5 is a cross-sectional view showing a laminate obtained after the sealing step shown in FIG. [Figure 6] FIG. 6 is a cross-sectional view showing a laminate obtained by carrying out a radiation exposure step on the laminate shown in FIG. 5. [Figure 7] 7 is a cross-sectional view showing a dicing position in a dicing step of the stacked body shown in FIG. 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] [Optical semiconductor element encapsulation sheet] The sheet for encapsulating an optical semiconductor element of the present invention includes at least a substrate and an encapsulation portion for encapsulating an optical semiconductor element, the encapsulation portion being provided on one surface of the substrate. In this specification, the sheet for encapsulating an optical semiconductor element refers to a sheet for encapsulating one or more optical semiconductor elements arranged on a substrate. In this specification, the term "encapsulating an optical semiconductor element" refers to embedding at least a part of the optical semiconductor element in the encapsulation portion.

[0029] The optical semiconductor element encapsulation sheet of the present invention may have a release liner in addition to the substrate and the encapsulation. In this case, the release liner is attached to the surface of the encapsulation part opposite to the substrate. The release liner is used as a protective material for the encapsulation part and is peeled off when encapsulating the optical semiconductor element. The release liner is not necessarily provided.

[0030] In addition, the optical semiconductor element encapsulation sheet of the present invention may have a surface protective film on the surface of the substrate (the surface opposite to the encapsulation portion). When an optical film described later is used as the substrate, the optical film can be protected until it is used. The surface protective film is not necessarily provided.

[0031] Hereinafter, an embodiment of the sheet for encapsulating optical semiconductor elements of the present invention will be described. FIG. 1 is a cross-sectional view showing an embodiment of the sheet for encapsulating optical semiconductor elements of the present invention. As shown in FIG. 1, the sheet for encapsulating optical semiconductor elements 1 can be used to encapsulate one or more optical semiconductor elements arranged on a substrate, and includes a substrate part 2, an encapsulating part 3, and a release liner 4. The encapsulating part 3 is provided on one side of the substrate part 2. The release liner 4 is attached to the surface of the encapsulating part 3 (the surface opposite to the side having the substrate part 2). In other words, the sheet for encapsulating optical semiconductor elements 1 includes the substrate part 2, the encapsulating part 3, and the release liner 4 in this order.

[0032] The optical semiconductor element encapsulation sheet preferably includes a layer having anti-glare and / or anti-reflection properties. With such a configuration, when the optical semiconductor device is tiled and applied to a display, the gloss of the display and the reflection of light can be suppressed, and the appearance of the display can be improved. An example of the layer having anti-glare properties is an anti-glare treated layer. An example of the layer having anti-reflection properties is an anti-reflection treated layer. The anti-glare treatment and the anti-reflection treatment can be performed by known or conventional methods. The layer having anti-glare properties and the layer having anti-reflection properties may be the same layer or different layers. The layer having anti-glare properties and / or anti-reflection properties may have only one layer, or two or more layers.

[0033] The layer having antiglare and / or antireflection properties may be any of a layer contained in the substrate, a layer contained in the sealing portion, or another layer not contained in the substrate or the sealing portion; however, it is preferably a layer contained in the substrate and / or the sealing portion, and more preferably a layer contained in the substrate.

[0034] The optical semiconductor element encapsulation sheet preferably includes a layer having a polyester resin and / or a polyimide resin as a main component (the component having the highest mass ratio among the constituent resins). With such a configuration, the optical semiconductor element encapsulation sheet has excellent heat resistance, and the thermal expansion of the optical semiconductor element encapsulation sheet can be suppressed in a high-temperature environment, improving dimensional stability. In addition, the sheet can be given rigidity, improving handling and retention. The layer having a polyester resin and / or a polyimide resin as a main component may have only one layer, or may have two or more layers.

[0035] The layer mainly composed of the polyester-based resin and / or the polyimide-based resin may be any of a layer contained in the base portion, a layer contained in the sealing portion, or another layer not contained in the base portion or the sealing portion; however, it is preferably a layer contained in the base portion and / or the sealing portion, and more preferably a layer contained in the base portion.

[0036] (Sealing part) The encapsulating portion has a resin layer (radiation curable resin layer) that has a property of being cured by irradiation with radiation, and an adhesive layer (non-radiation curable adhesive layer) that does not have a property of being cured by irradiation with radiation. The non-radiation curable adhesive layer is located on the surface of the encapsulating portion that faces the optical semiconductor element when encapsulating the optical semiconductor element. Specifically, the non-radiation curable adhesive layer is located on the surface of the sheet for encapsulating optical semiconductor elements that faces the optical semiconductor element when encapsulating the optical semiconductor element (the sheet surface excluding the release liner when a release liner is provided). For example, in the sheet for encapsulating optical semiconductor elements 1 shown in FIG. 1, the encapsulating portion 3 is composed of a radiation curable resin layer 31 and a non-radiation curable adhesive layer 32. The non-radiation curable adhesive layer 32 is located on the surface of the sheet for encapsulating optical semiconductor elements 1 opposite to the substrate portion 2, excluding the release liner 4.

[0037] By positioning the radiation non-curable pressure-sensitive adhesive layer on the surface, when the sheet for encapsulating an optical semiconductor element encapsulates an optical semiconductor element, the radiation non-curable pressure-sensitive adhesive layer has excellent adhesion to the optical semiconductor element and the substrate, and the sheet for encapsulating an optical semiconductor element is excellent. After encapsulation, the radiation curable resin layer is cured by irradiation with radiation, and the adhesion of the side surface of the sheet for encapsulation decreases. As a result, the adhesion between the encapsulation parts of adjacent optical semiconductor devices in a tiling state is low, and when adjacent optical semiconductor devices are separated from each other, the sheet is less likely to be damaged or the sheets of adjacent optical semiconductor devices are less likely to adhere to each other. In addition, the substrate part serves as a support for the encapsulation part, and the sheet for encapsulating an optical semiconductor element has excellent handleability by including the substrate part. In addition, when dicing after encapsulating an optical semiconductor device with the sheet for encapsulating an optical semiconductor element, the stickiness of the diced part can be further suppressed, and an optical semiconductor device with a good appearance can be produced.

[0038] In the sealing part, the radiation non-curable adhesive layer and the radiation curable resin layer are laminated. The radiation non-curable adhesive layer and the radiation curable resin layer may be laminated directly without any other layer, or may be laminated via another layer. The radiation non-curable adhesive layer and the radiation curable resin layer may each be a single layer, or may be multiple layers having the same composition or different thickness. When the sealing part has at least one of the radiation non-curable adhesive layer and the radiation curable resin layer in a plurality of layers, the multiple layers may be laminated continuously or may be laminated via another layer. When the sealing part has multiple layers of the radiation non-curable adhesive layer, it is sufficient that one layer is present on the surface opposite to the substrate part of the sheet for sealing optical semiconductor elements, and the position of the other radiation non-curable adhesive layer is not particularly limited.

[0039] The ratio of the thickness (total thickness) of the radiation curable resin layer to the thickness (total thickness) of the non-radiation curable adhesive layer [thickness of radiation curable resin layer / thickness of radiation non-curable adhesive layer] is preferably 0.1 or more, more preferably 0.8 or more, even more preferably more than 1.0, and particularly preferably 4 or more. When the ratio is 0.1 or more, damage to the sheet or adhesion of the sheets of adjacent optical semiconductor devices is less likely to occur when the adjacent optical semiconductor devices are separated from each other. In addition, the ratio is preferably 200 or less, more preferably 150 or less.

[0040] The radiation curable resin layer is preferably thicker than the non-radiation curable adhesive layer. With this configuration, the low adhesion between the radiation curable resin layers in adjacent optical semiconductor devices after curing becomes dominant over the high adhesion between the radiation non-curable adhesive layers in adjacent optical semiconductor devices in a tiling state, so that the adhesion between the sealing parts is further lower, and when the adjacent optical semiconductor devices are separated from each other, the sheet is less likely to be damaged or the sheets of the adjacent optical semiconductor devices are less likely to adhere to each other. In addition, when the optical semiconductor device is produced by sealing the optical semiconductor element with the sheet for sealing the optical semiconductor element and then dicing, the stickiness of the diced part can be further suppressed, and an optical semiconductor device with a good appearance can be produced. In addition, when there are multiple radiation curable resin layers or multiple radiation non-curable adhesive layers, the thickness is the total thickness (total thickness) of the multiple layers.

[0041] The thickness of the non-radiation curable pressure-sensitive adhesive layer located on the surface of the sheet for encapsulating optical semiconductor elements (i.e., the surface of the encapsulation portion) is preferably 1 μm or more, more preferably 4 μm or more, and even more preferably 15 μm or more. When the thickness is 1 μm or more, the sheet for encapsulating optical semiconductor elements has better adhesion to the optical semiconductor elements and the substrate. The thickness is preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 200 μm or less. When the thickness is 500 μm or less, when adjacent optical semiconductor devices are separated from each other, the sheet is less likely to be damaged or the sheets of adjacent optical semiconductor devices are less likely to adhere to each other. In addition, when dicing the optical semiconductor device, stickiness of the diced portion can be further suppressed, and an optical semiconductor device with good appearance can be produced.

[0042] The thickness (total thickness) of the radiation curable resin layer is preferably 20 to 800 μm, more preferably 30 to 700 μm, and even more preferably 50 to 600 μm. If the thickness is 20 μm or more, damage to the sheet or adhesion of the sheets of adjacent optical semiconductor devices is less likely to occur when the adjacent optical semiconductor devices are separated from each other. If the thickness is 800 μm or less, the thickness of the sealing portion can be reduced, and the optical semiconductor device can be made thinner.

[0043] The optical semiconductor element encapsulation sheet preferably includes a radiation curable resin layer having the thickest thickness among all layers constituting the encapsulation part. A layer in which multiple layers of the same composition are directly laminated is considered as one layer. In addition, when there are two or more thickest layers, all of the layers correspond to the thickest layer.

[0044] The ratio of the thickness (total thickness) of the radiation curable resin layer to the total thickness (excluding the release liner and surface protective film) of the sheet for encapsulating optical semiconductor elements (100%) is preferably 5 to 90%, more preferably 10 to 85%, and even more preferably 40 to 80%. When the ratio is 5% or more, damage to the sheet or adhesion of the sheets of adjacent optical semiconductor devices is less likely to occur when the adjacent optical semiconductor devices are separated from each other. When the thickness is 90% or less, the thickness of the encapsulation portion can be reduced, and the optical semiconductor device can be made thinner.

[0045] The hardness of the radiation curable resin layer at a cross section of the layer after curing, measured by a nanoindentation method at a temperature of 23°C, is preferably 1.4 MPa or more, more preferably 11.0 MPa or more, and even more preferably 63.0 MPa or more. The hardness by the nanoindentation method is determined by continuously measuring the load and indentation depth on an indenter when the indenter is pressed into a target surface, during loading and unloading, and from the applied load-indentation depth curve obtained. If the hardness is 1.4 MPa or more, the radiation curable resin layer has an appropriate hardness after curing, and when adjacent optical semiconductor devices are separated from each other in a tiling state, damage to the sheet and adhesion of the sheets of adjacent optical semiconductor devices are even less likely to occur.

[0046] The radiation-curable resin layer has radiation curability. Examples of the radiation include electron beams, ultraviolet rays, α rays, β rays, γ rays, and X-rays.

[0047] Examples of the radiation-curable resin layer include a layer containing a base polymer and a radiation-polymerizable monomer component or oligomer component having a functional group such as a radiation-polymerizable carbon-carbon double bond, and a layer containing a polymer having a radiation-polymerizable functional group as a base polymer.

[0048] Examples of the resin constituting the radiation-curable resin layer include known or commonly used radiation-curable resins, such as acrylic resins, urethane acrylate resins, epoxy resins, epoxy acrylate resins, oxetane resins, silicone resins, silicone acrylic resins, polyester resins, etc. Only one type of the above resins may be used, or two or more types may be used.

[0049] The radiation-curable resin layer is preferably a resin layer having adhesive properties, i.e., a radiation-curable pressure-sensitive adhesive layer. With such a configuration, when sealing an optical semiconductor element, the optical semiconductor element can be easily embedded, and the adhesion between the substrate and the non-radiation-curable pressure-sensitive adhesive layer located on the optical semiconductor element side surface before radiation curing is excellent, resulting in superior sealing of the optical semiconductor element.

[0050] The adhesive forming the non-radiation curable adhesive layer may be a known or commonly used pressure-sensitive adhesive that is not radiation curable, i.e. does not contain a compound having radiation curability. However, it may contain a small amount of a compound having radiation curability that is unavoidably transferred from another laminated layer. Examples of the adhesive include acrylic adhesives, rubber adhesives (natural rubber, synthetic rubber, a mixture of these, etc.), silicone adhesives, polyester adhesives, urethane adhesives, polyether adhesives, polyamide adhesives, and fluorine adhesives. Only one type of the adhesive may be used, or two or more types may be used.

[0051] The sealing part may have layers other than the radiation curable resin layer and the non-radiation curable pressure-sensitive adhesive layer, provided that the ratio of the total thickness of the radiation curable resin layer and the non-radiation curable pressure-sensitive adhesive layer to the 100% thickness of the sealing part is preferably 70% or more, more preferably 80% or more, even more preferably 90% or more, and particularly preferably 96% or more.

[0052] The sealing part may include a layer containing a colorant. With such a configuration, when the optical semiconductor device is tiled and applied to a display, it is possible to suppress color mixing of light emitted by each optical semiconductor element when the optical semiconductor device is in use, and to adjust the appearance of the display when the optical semiconductor device is not in use. The layer containing the colorant may be only one layer, or may have two or more layers.

[0053] The layer containing the colorant may be the radiation curable resin layer, the non-radiation curable adhesive layer, or a layer other than these. However, it is preferable that the radiation curable resin layer and / or the non-radiation curable adhesive layer is a layer containing a colorant, and it is more preferable that the non-radiation curable adhesive layer is a layer containing a colorant.

[0054] The above-mentioned colorant is preferably a black colorant. As the above-mentioned black colorant, a known or conventional colorant (pigment, dye, etc.) for providing black color can be used, and examples thereof include carbon black (furnace black, channel black, acetylene black, thermal black, lamp black, pine smoke, etc.), graphite, copper oxide, manganese dioxide, aniline black, perylene black, titanium black, cyanine black, activated carbon, ferrite (non-magnetic ferrite, magnetic ferrite, etc.), magnetite, chromium oxide, iron oxide, molybdenum disulfide, chromium complex, anthraquinone colorant, zirconium nitride, etc. The black colorant may be used alone or in combination with two or more kinds. In addition, a colorant that functions as a black colorant may be used by combining and blending colorants that provide a color other than black.

[0055] (Base material part) The substrate serves as a support for the encapsulation portion, and the substrate provides the sheet for encapsulating optical semiconductor elements with excellent handling properties. The substrate may be a single layer, or may be a multilayer having the same or different compositions, thicknesses, etc. When the substrate is a multilayer, each layer may be bonded to another layer such as a pressure-sensitive adhesive layer. The substrate layer used in the substrate is a portion that is attached to a substrate having an optical semiconductor element together with the encapsulation portion when the sheet for encapsulating optical semiconductor elements is used to encapsulate the optical semiconductor element, and the release liner that is peeled off when the sheet for encapsulating optical semiconductor elements is used (attached) and the surface protection film that merely protects the surface of the substrate are not included in the "substrate".

[0056] Examples of the substrate layer constituting the substrate part include glass and plastic substrates (particularly, plastic films), etc. Examples of the resin constituting the plastic substrate include low-density polyethylene, linear low-density polyethylene, medium-density polyethylene, high-density polyethylene, very low-density polyethylene, random copolymer polypropylene, block copolymer polypropylene, homopolypropylene, polybutene, polymethylpentene, ionomer, ethylene-(meth)acrylic acid copolymer, ethylene-(meth)acrylic acid ester (random, alternating) copolymer, ethylene-vinyl acetate copolymer (EVA), ethylene-propylene copolymer, cyclic olefin polymer, ethylene-butene copolymer, ethylene-hexene copolymer, etc. Examples of the resin include polyolefin resin, polyurethane, polyester such as polyethylene terephthalate (PET), polyethylene naphthalate, polybutylene terephthalate (PBT), polycarbonate, polyimide resin, polyether ether ketone, polyetherimide, polyamide such as aramid and fully aromatic polyamide, polyphenyl sulfide, fluororesin, polyvinyl chloride, polyvinylidene chloride, cellulose resin such as triacetyl cellulose (TAC), silicone resin, acrylic resin such as polymethyl methacrylate (PMMA), polysulfone, polyarylate, polyvinyl acetate, etc. Only one of the above resins may be used, or two or more of them may be used.

[0057] The substrate layer may be various optical films such as an antireflection (AR) film, a polarizing plate, a retardation plate, etc. When the substrate portion has an optical film, the optical semiconductor element encapsulation sheet can be applied directly to an optical member.

[0058] The plastic film preferably contains a polyester resin and / or a polyimide resin as a main component (the component with the highest mass ratio among the constituent resins). With such a configuration, the sheet for encapsulating an optical semiconductor element has excellent heat resistance, and the thermal expansion of the sheet for encapsulating an optical semiconductor element in a high-temperature environment can be suppressed, improving dimensional stability. In addition, the rigidity of the sheet can be imparted, improving handling and retention.

[0059] The thickness of the plastic film is preferably 20 to 200 μm, more preferably 40 to 150 μm. When the thickness is 20 μm or more, the supportability and handleability of the optical semiconductor element encapsulation sheet are further improved. When the thickness is 200 μm or less, the thickness of the optical semiconductor element encapsulation sheet can be reduced, and the optical semiconductor device can be made thinner.

[0060] The substrate preferably includes a plastic film mainly composed of a polyester resin and / or a polyimide resin, and an optical film. Optical films such as polarizing plates generally tend to be poor in supportability and handling, and by using them in combination with the plastic film, the advantages of both can be utilized. In this case, it is particularly preferable that the plastic film is on the sealing part side of the substrate.

[0061] The substrate preferably includes a layer having antiglare properties and / or antireflection properties. The layer having antiglare properties and / or antireflection properties is obtained as the antiglare treatment layer or the antireflection treatment layer by, for example, performing antiglare treatment and / or antireflection treatment on at least one surface of the substrate layer. The antiglare treatment layer and the antireflection treatment layer may be the same layer or different layers. The antiglare treatment and the antireflection treatment can be performed by known or conventional methods.

[0062] The surface of the substrate on the side where the sealing portion is provided may be subjected to a surface treatment such as a physical treatment such as corona discharge treatment, plasma treatment, sand mat processing treatment, ozone exposure treatment, flame exposure treatment, high-voltage shock exposure treatment, ionizing radiation treatment, etc.; a chemical treatment such as chromate treatment; or an easy-adhesion treatment using a coating agent (primer), etc., for the purpose of improving adhesion and retention with the sealing portion. The surface treatment for improving adhesion is preferably applied to the entire surface of the substrate on the side of the sealing portion.

[0063] 1, the substrate 2 is a multilayered structure including an optical film 21 and a plastic film 23, and the optical film 21 and the plastic film 23 are bonded together via an adhesive layer 22. The surface of the optical film 21 facing the plastic film 23 has been subjected to anti-glare treatment and anti-reflection treatment.

[0064] The thickness of the substrate is preferably 5 μm or more, more preferably 10 μm or more, from the viewpoint of excellent support function and surface scratch resistance, and is preferably 300 μm or less, more preferably 200 μm or less, from the viewpoint of excellent transparency.

[0065] (Release liner) The release liner is an element for covering and protecting the surface of the encapsulating portion, and is peeled off from the sheet when the optical semiconductor element encapsulating sheet is attached to a substrate on which an optical semiconductor element is arranged.

[0066] Examples of the release liner include polyethylene terephthalate (PET) film, polyethylene film, polypropylene film, plastic films and papers whose surfaces are coated with a release agent such as a fluorine-based release agent or a long-chain alkyl acrylate-based release agent.

[0067] The thickness of the release liner is, for example, 10 to 200 μm, preferably 15 to 150 μm, and more preferably 20 to 100 μm. When the thickness is 10 μm or more, the release liner is less likely to break due to incisions during processing. When the thickness is 200 μm or less, the release liner is more easily peeled off from the sealed portion during use.

[0068] (Optical semiconductor element encapsulation sheet) The ratio of the total thickness of the substrate and the encapsulation portion in the optical semiconductor element encapsulation sheet is preferably 80% or more, more preferably 90% or more, relative to 100% of the thickness of the optical semiconductor element encapsulation sheet (excluding the release liner and the surface protection film). In addition, the ratio of the thickness from the substrate surface to the encapsulation portion surface, including the substrate and the encapsulation portion, is preferably within the above range.

[0069] The total thickness of the substrate and the encapsulating portion in the optical semiconductor element encapsulating sheet is preferably 100 to 900 μm, more preferably 200 to 800 μm. In addition, the thickness from the substrate surface to the encapsulating portion surface, including the substrate and the encapsulating portion, is preferably within the above range.

[0070] An embodiment of the method for producing a sheet for encapsulating an optical semiconductor element of the present invention will be described. For example, the sheet for encapsulating an optical semiconductor element 1 shown in FIG. 1 can be produced by the following method. First, a radiation curable resin layer 31 is formed on a plastic film 23 constituting a substrate portion 2. The radiation curable resin layer 31 can be produced by applying a resin composition for forming the radiation curable resin layer 31 to one side of the plastic film 23 to form a resin composition layer, and then performing curing other than radiation irradiation, such as desolvation by heating or heat curing, to solidify the resin composition layer. When the thickness of the radiation curable resin layer 31 is to be increased, a radiation curable resin layer produced in the same manner on the release-treated surface of a release liner may be laminated on the radiation curable resin layer formed on the plastic film 23.

[0071] The resin composition forming the radiation curable resin layer may be in any form as long as it does not impair the radiation curability of the radiation curable resin layer. For example, the pressure-sensitive adhesive composition may be an emulsion type, a solvent type (solution type), a hot melt type, etc. Among these, the solvent type is preferred because it is easy to obtain a pressure-sensitive adhesive layer with excellent productivity.

[0072] Meanwhile, a non-radiation-curable adhesive layer 32 is formed on the release-treated surface of a release liner 4 prepared separately. The non-radiation-curable adhesive layer 32 can be produced by applying an adhesive composition for forming the non-radiation-curable adhesive layer 32 onto the release-treated surface of the release liner 4 to form an adhesive composition layer, and then heating to remove the solvent and cure the adhesive composition layer to solidify it. The non-radiation-curable adhesive layer is then laminated on the radiation-curable resin layer. In this manner, a laminate having a configuration of [plastic film 23 / radiation-curable resin layer 31 / non-radiation-curable adhesive layer 32 / release liner 4] is obtained.

[0073] The adhesive composition forming the non-radiation curable adhesive layer may be in any form. For example, the adhesive composition may be an emulsion type, a solvent type (solution type), an active energy ray curable type, a hot melt type, etc. Among them, the solvent type and the active energy ray curable type adhesive composition are preferred because they are easy to obtain an adhesive layer with excellent productivity.

[0074] On the other hand, a laminate of an optical film 21 and a pressure-sensitive adhesive layer 22 is prepared. Specifically, for example, the pressure-sensitive adhesive layer 22 is formed on the release-treated surface of a separately prepared release liner in the same manner as the radiation-non-curable pressure-sensitive adhesive layer 32, and then the optical film 21 is laminated on the pressure-sensitive adhesive layer 22. The release liner is then peeled off to expose the pressure-sensitive adhesive layer 22, which is then laminated to the surface of the plastic film 23 of the laminate on which the radiation-curable resin layer 31 is not formed. For example, known or commonly used coating methods can be used to apply the resin composition or pressure-sensitive adhesive composition, and examples of such methods include roll coating, screen coating, and gravure coating. In addition, the lamination of various layers can be performed using a known roller or laminator. In this manner, the sheet 1 for encapsulating optical semiconductor elements shown in FIG. 1 can be prepared.

[0075] The method for producing the optical semiconductor element encapsulation sheet of the present invention is not limited to the above-mentioned method. When the substrate portion is composed of multiple layers, the substrate portion can be prepared first, and then an appropriate combination of a radiation curable resin layer and a non-radiation curable pressure-sensitive adhesive layer can be laminated on the substrate portion in that order, so that the non-radiation curable pressure-sensitive adhesive layer is located on the surface.

[0076] The optical semiconductor device can be obtained by laminating the radiation non-curable pressure-sensitive adhesive layer on a substrate on which an optical semiconductor element is arranged using the sheet for sealing an optical semiconductor device of the present invention, and sealing the optical semiconductor element with the sealing part. Specifically, first, the release liner is peeled off from the sheet for sealing an optical semiconductor element of the present invention to expose the radiation non-curable pressure-sensitive adhesive layer. Then, the exposed surface of the sheet for sealing an optical semiconductor element of the present invention is laminated to the substrate surface on which the optical semiconductor element is arranged of an optical member comprising a substrate and an optical semiconductor element (preferably a plurality of optical semiconductor elements) arranged on the substrate, and when the optical member comprises a plurality of optical semiconductor elements, the radiation non-curable pressure-sensitive adhesive layer is further arranged so as to fill the gaps between the plurality of optical semiconductor elements, and the plurality of optical semiconductor elements are collectively sealed. In this way, the optical semiconductor element can be sealed using the sheet for sealing an optical semiconductor device of the present invention. The optical semiconductor element may also be sealed by laminating the sheet for sealing an optical semiconductor device of the present invention under a reduced pressure environment or while applying pressure. Examples of such methods include those disclosed in JP-A-2016-29689 and JP-A-6-97268.

[0077] [Optical semiconductor device] An optical semiconductor device can be produced using the sheet for encapsulating an optical semiconductor element of the present invention. The optical semiconductor device produced using the sheet for encapsulating an optical semiconductor element of the present invention comprises a substrate, an optical semiconductor element disposed on the substrate, and a cured product obtained by curing the sheet for encapsulating an optical semiconductor element of the present invention, which encapsulates the optical semiconductor element. The cured product is a cured product obtained by curing the sheet for encapsulating an optical semiconductor element of the present invention by irradiation with radiation, and specifically comprises a cured encapsulating layer obtained by curing the radiation-curable resin layer in the sheet for encapsulating an optical semiconductor element of the present invention by irradiation with radiation.

[0078] Examples of the optical semiconductor element include light emitting diodes (LEDs) such as blue light emitting diodes, green light emitting diodes, red light emitting diodes, and ultraviolet light emitting diodes.

[0079] In the above-mentioned optical semiconductor device, the sheet for encapsulating optical semiconductor elements of the present invention has excellent conformability to irregularities when the optical semiconductor elements are convex parts and the gaps between multiple optical semiconductor elements are concave parts, and has excellent embeddability of the optical semiconductor elements, and therefore it is preferable that the sheet encapsulates multiple optical semiconductor elements collectively.

[0080] FIG. 2 shows an embodiment of an optical semiconductor device using the optical semiconductor element encapsulation sheet 1 shown in FIG. 1. The optical semiconductor device 10 shown in FIG. 2 includes a substrate 5, a plurality of optical semiconductor elements 6 arranged on one surface of the substrate 5, and a cured product 1' of the optical semiconductor element encapsulation sheet that encapsulates the optical semiconductor elements 6. The cured product 1' of the optical semiconductor element encapsulation sheet is formed by peeling the release liner 4 from the optical semiconductor element encapsulation sheet 1 and curing the radiation curable resin layer 31 by radiation irradiation to form a cured encapsulation layer 31'. The plurality of optical semiconductor elements 6 are encapsulated together in the encapsulation section. The non-radiation curable pressure-sensitive adhesive layer 32 in the encapsulation section is in close contact with the optical semiconductor elements 6 and the substrate 5 while following the uneven shape formed by the plurality of optical semiconductor elements 6, and embeds the optical semiconductor elements 6.

[0081] 2, the optical semiconductor element 6 is completely embedded and sealed in the non-radiation-curable pressure-sensitive adhesive layer 32, and is indirectly sealed by the cured sealing layer 31'. The optical semiconductor device is not limited to this embodiment, and may be such that a part of the optical semiconductor element 6 protrudes from the non-radiation-curable pressure-sensitive adhesive layer 32 and is embedded in the cured sealing layer 31', such that the optical semiconductor element 6 is completely embedded and sealed between the non-radiation-curable pressure-sensitive adhesive layer 32 and the cured sealing layer 31'.

[0082] As described above, the optical semiconductor device encapsulates the optical semiconductor element with the non-radiation-curable pressure-sensitive adhesive layer and the cured sealing layer which is a cured product of the radiation-curable resin layer. Therefore, the optical semiconductor element is in close contact with the non-radiation-curable pressure-sensitive adhesive layer, providing excellent sealing properties for the optical semiconductor element, and the side surface of the cured sealing layer has low adhesion. Therefore, when adjacent optical semiconductor devices are separated from each other in a tiled state, they can be easily separated, and loss of the sheet or adhesion of the sheets of adjacent optical semiconductor devices is unlikely to occur.

[0083] The optical semiconductor device may be one in which individual optical semiconductor devices are tiled, that is, the optical semiconductor device may be one in which a plurality of optical semiconductor devices are arranged in a tiled shape in a planar direction.

[0084] Fig. 3 shows one embodiment of an optical semiconductor device fabricated by arranging a plurality of optical semiconductor devices. The optical semiconductor device 20 shown in Fig. 3 has a plurality of optical semiconductor devices 10 arranged in a tiled pattern (tiling) in the planar direction, 4 in the vertical direction and 4 in the horizontal direction, for a total of 16 devices. At the boundary 20a between two adjacent optical semiconductor devices 10, the optical semiconductor devices 10 are adjacent to each other, but they can be easily separated, and damage to the side surface of the sealing portion and adhesion of the resin that has been damaged on the side surface of the sealing portion from one adjacent optical semiconductor device to the other is unlikely to occur.

[0085] The optical semiconductor device is preferably a backlight for a liquid crystal screen, and particularly preferably a full-surface direct-light type backlight. Moreover, the backlight can be combined with a display panel to form an image display device. When the optical semiconductor device is a backlight for a liquid crystal screen, the optical semiconductor element is an LED element. For example, in the backlight, a metal wiring layer for sending a light emission control signal to each LED element is laminated on the substrate. Each LED element emitting light of each color of red (R), green (G), and blue (B) is alternately arranged on the substrate of the display panel via a metal wiring layer. The metal wiring layer is formed of a metal such as copper, and reflects the light emitted by each LED element, thereby reducing the visibility of the image. Moreover, the light emitted by each LED element of each color of RGB is mixed, reducing the contrast.

[0086] Moreover, the optical semiconductor device is preferably a self-luminous display device. Moreover, the self-luminous display device can be combined with a display panel as necessary to form an image display device. When the optical semiconductor device is a self-luminous display device, the optical semiconductor element is an LED element. The self-luminous display device can be an organic electroluminescence (organic EL) display device. For example, in the self-luminous display device, a metal wiring layer for sending a light emission control signal to each LED element is laminated on the substrate. Each LED element emitting light of each color, red (R), green (G), and blue (B), is alternately arranged on the substrate via a metal wiring layer. The metal wiring layer is formed of a metal such as copper, and the light emission degree of each LED element is adjusted to display each color.

[0087] The optical semiconductor element encapsulation sheet of the present invention can be used in an optical semiconductor device that is folded for use, for example, an optical semiconductor device having a foldable image display device (flexible display) (particularly, a foldable image display device (foldable display)). Specifically, it can be used in a foldable backlight and a foldable self-luminous display device.

[0088] The sheet for encapsulating an optical semiconductor element of the present invention has excellent embeddability for an optical semiconductor element, and therefore can be preferably used when the optical semiconductor device is either a mini LED display device or a micro LED display device.

[0089] [Method of manufacturing optical semiconductor device] The optical semiconductor device can be produced, for example, by a production method including at least a dicing step of dicing a laminate including a substrate, an optical semiconductor element disposed on the substrate, and a cured product obtained by curing the radiation-curable resin layer of the sheet for encapsulating an optical semiconductor element of the present invention, which encapsulates the optical semiconductor element, to obtain an optical semiconductor device. The cured product is a cured product obtained by curing the sheet for encapsulating an optical semiconductor element of the present invention by irradiation with radiation, and specifically includes a cured encapsulating layer obtained by curing the radiation-curable resin layer in the sheet for encapsulating an optical semiconductor element of the present invention by irradiation with radiation.

[0090] When the radiation curable resin layer is irradiated with radiation and cured, curing is inhibited on the side where oxygen is present, and curing is likely to be insufficient. In contrast, according to the above-mentioned manufacturing method including the dicing step, for a laminate including a cured product of a sheet for encapsulating optical semiconductor elements, including a cured encapsulating layer obtained by curing the radiation curable resin layer by irradiation with radiation, the side end portion that is insufficiently cured in the dicing step is cut off and removed, thereby obtaining an optical semiconductor device in which an area that has been sufficiently cured and has reduced adhesion is exposed on the side. In the optical semiconductor device manufactured in this way, the adhesion of the side surface of the radiation curable resin layer after curing is sufficiently reduced, so that when adjacent optical semiconductor devices are separated from each other in a tiling state, the sheet is unlikely to be damaged or the sheets of adjacent optical semiconductor devices are unlikely to adhere to each other.

[0091] The above-mentioned manufacturing method may further include a radiation exposure step of irradiating a laminate comprising the above-mentioned substrate, an optical semiconductor element disposed on the above-mentioned substrate, and the sheet for encapsulating an optical semiconductor element that encapsulates the optical semiconductor element with radiation to cure the radiation-curable resin layer and obtain the cured product.

[0092] The manufacturing method may include, prior to the radiation exposure step, a sealing step of bonding the sheet for sealing an optical semiconductor element to the optical semiconductor element provided on the substrate to seal the optical semiconductor element with the sealing portion.

[0093] The manufacturing method may further include a tiling step of arranging the multiple optical semiconductor devices obtained in the dicing step so that they are in contact with each other in a planar direction. Hereinafter, the manufacturing method of the optical semiconductor device 10 shown in FIG. 2 and the optical semiconductor device 20 shown in FIG. 3 will be described with reference to them as appropriate.

[0094] (Sealing process) In the above-mentioned encapsulation step, the sheet for encapsulating optical semiconductor elements of the present invention is attached to a substrate on which an optical semiconductor element is arranged, and the optical semiconductor element is encapsulated by the encapsulation portion. In the above-mentioned encapsulation step, specifically, as shown in FIG. 4, the radiation non-curable adhesive layer 32 of the sheet for encapsulating optical semiconductor elements 1 from which the release liner 4 has been peeled is disposed so as to face the surface of the substrate 5 on which the optical semiconductor element 6 is arranged, and the sheet for encapsulating optical semiconductor elements 1 is attached to the surface of the substrate 5 on which the optical semiconductor element 6 is arranged, and the optical semiconductor element 6 is embedded in the encapsulation portion 3 as shown in FIG. 5. As shown in FIG. 4, the substrate 5 used for encapsulation extends wider in the planar direction than the substrate 5 in the optical semiconductor device 10 shown in FIG. 2, and the optical semiconductor element 6 is not arranged near the end of the substrate 5. In addition, the sheet for encapsulating optical semiconductor elements 1 to be affixed extends wider in the planar direction than the substrate 5 to be affixed. That is, the surface area of ​​the sheet for encapsulating optical semiconductor elements 1 to be affixed in the encapsulation step facing the substrate 5 is larger than the surface area of ​​the substrate 5 to be affixed in the encapsulation step facing the sheet for encapsulating optical semiconductor elements 1. This is because the area of ​​the laminate of the sheet 1 for encapsulating an optical semiconductor element and the substrate 5 that will be used for the optical semiconductor device is sufficiently cured in the subsequent radiation exposure process, while the areas near the edges of the sheet 1 for encapsulating an optical semiconductor element and the substrate 5 that may not be sufficiently cured are diced and removed in the subsequent dicing process.

[0095] The temperature during the lamination is, for example, within a range of room temperature to 110°C. Furthermore, reduced pressure or pressure may be applied during the lamination. The reduced pressure or pressure can prevent the formation of voids between the encapsulating portion and the substrate or the optical semiconductor element. Furthermore, in the encapsulation step, it is preferable to laminate the optical semiconductor element encapsulation sheet under reduced pressure and then apply pressure. When reduced pressure is applied, the pressure is, for example, 1 to 100 Pa, and the depressurization time is, for example, 5 to 600 seconds. When pressurized, the pressure is, for example, 0.05 to 0.5 MPa, and the depressurization time is, for example, 5 to 600 seconds.

[0096] (Radiation irradiation process) In the radiation irradiation step, a laminate (for example, a laminate obtained in the encapsulation step) in which the sheet for encapsulating an optical semiconductor element is attached to the substrate on which the optical semiconductor element is disposed is irradiated with radiation to cure the radiation curable resin layer. Specifically, in the radiation irradiation step, as shown in FIG. 6, the radiation curable resin layer 31 is cured to form a cured encapsulation layer 31', and a cured product 1' of the sheet for encapsulating an optical semiconductor element 1 is obtained. As described above, examples of the radiation include electron beams, ultraviolet rays, α rays, β rays, γ rays, and X-rays. Among these, ultraviolet rays are preferred. The temperature during radiation irradiation is, for example, within the range of room temperature to 100°C, and the irradiation time is, for example, 1 minute to 1 hour.

[0097] (Dicing process) In the dicing step, a laminate (e.g., a laminate having undergone the radiation irradiation step) including a substrate, an optical semiconductor element disposed on the substrate, and a cured product of the optical semiconductor element encapsulation sheet of the present invention that encapsulates the optical semiconductor element is diced. Here, in the laminate to be subjected to the dicing step, the cured product 1' of the optical semiconductor element encapsulation sheet and the substrate 5 extend wider in the planar direction than the optical semiconductor device 10 finally obtained, as described above. Then, in the dicing step, the side end portions of the cured product of the optical semiconductor element encapsulation sheet and the substrate are diced and removed. Specifically, dicing is performed at the position of the dashed line shown in FIG. 7 to remove the side end portions. The dicing can be performed by a known or conventional method, for example, a method using a dicing blade or laser irradiation. In this manner, for example, the optical semiconductor device 10 shown in FIG. 2 can be manufactured.

[0098] Here, in the above-mentioned manufacturing method, it is important to perform dicing in a state where the radiation curable resin layer is cured, for example, by undergoing the above-mentioned radiation irradiation step. If dicing is performed in a state where the radiation curable resin layer is not cured, when the side end of the sheet for sealing optical semiconductor elements is to be pulled apart and removed after dicing, the adhesion between the radiation curable resin layers in the side end to be removed and the remaining optical semiconductor device is high, and they adhere to each other and attract each other, which may cause defects such as defects in the radiation curable resin layer in the remaining optical semiconductor device, or a part of the radiation curable resin layer in the side end to be removed being transferred and attached to the remaining optical semiconductor device. In contrast, by providing the above-mentioned dicing step in which dicing is performed in a state where the radiation curable resin layer is cured, the radiation curable resin layer is cured to become a cured sealing layer, so that the adhesion of the side of the diced part is low, and the occurrence of the above-mentioned defects can be suppressed.

[0099] Also, when curing the radiation-curable resin layer by irradiating it with radiation, curing is inhibited on the side surface where oxygen is present, and it is likely to become insufficient. On the other hand, according to the above manufacturing method including the above dicing process, in the state where the above radiation-curable resin layer is cured, by cutting off and removing the end part where curing is insufficient in the above dicing process, an optical semiconductor device can be obtained in which the side surface is sufficiently cured and the adhesion is reduced. The optical semiconductor device manufactured in this way has a sufficiently reduced adhesion on the side surface after curing the radiation-curable resin layer. Therefore, when separating adjacent optical semiconductor devices in a tiling state, it is less likely to cause sheet defects or adhesion of the sheet of the adjacent optical semiconductor device. On the other hand, when the above dicing process is not provided, during tiling, since the side surface where curing is insufficient comes into contact with the adjacent optical semiconductor device, when trying to separate adjacent optical semiconductor devices, the side surfaces adhere to each other and attract, and defects may occur in the radiation-curable resin layer in one optical semiconductor device, or a part of the radiation-curable resin layer in the other optical semiconductor device may be transferred and adhered to one optical semiconductor device.

[0100] (Tiling process) In the above tiling process, a plurality of optical semiconductor devices obtained in the above dicing process are arranged in contact with each other in a planar direction for tiling. In this way, for example, the optical semiconductor device 20 shown in FIG. 3 can be manufactured. The optical semiconductor device obtained by tiling has excellent sealing properties of the optical semiconductor element, and when separating adjacent optical semiconductor devices, it is less likely to cause sheet defects or adhesion of the sheet of the adjacent optical semiconductor device.

Example

[0101] The present invention will be described in more detail with reference to the following examples, but the present invention is not limited to these examples in any way.

[0102] Example 1 <TAC film / Binder adhesive layer> As monomer components, 69.7 parts by mass of 2-ethylhexyl acrylate (2EHA), 10 parts by mass of 2-methoxyethyl acrylate (MEA), 13 parts by mass of 2-hydroxyethyl acrylate (HEA), 6 parts by mass of N-vinyl-2-pyrrolidone (NVP), 1.3 parts by mass of N-hydroxyethylacrylamide (HEAA), 0.1 part by mass of 2,2'-azobisisobutyronitrile as a polymerization initiator, and 200 parts by mass of ethyl acetate as a polymerization solvent were charged into a separable flask and stirred for 1 hour while introducing nitrogen gas. In this way, after removing oxygen in the polymerization system, the temperature was raised to 63 °C and reacted for 10 hours, and then ethyl acetate was added to obtain an acrylic polymer solution with a solid content concentration of 30% by mass. With respect to 100 parts by mass of the above acrylic polymer, 0.2 part by mass of an isocyanate-based crosslinking agent (trade name "Takenate D110N", manufactured by Mitsui Chemicals, Inc.) as a crosslinking agent, 0.15 part by mass of γ-glycidoxypropyltrimethoxysilane (trade name "KBM-403", manufactured by Shin-Etsu Chemical Co., Ltd.) as a silane coupling agent, and 0.2 part by mass of a polyol obtained by adding propylene oxide to ethylenediamine (trade name "EDP-300", manufactured by ADEKA Corporation) as a crosslinking accelerator were added to prepare an adhesive composition (solution). Next, the above adhesive composition (solution) was applied onto the release-treated surface of a release liner (separator) (trade name "MRF38", manufactured by Mitsubishi Chemical Corporation) so that the thickness after drying would be 25 μm, and heated and dried at 60 °C for 1 minute and at 155 °C for 1 minute under normal pressure to obtain a double-sided adhesive sheet as a binder adhesive layer. Then, using a hand roller, the adhesive surface of the binder adhesive layer was bonded to the untreated surface of a triacetylcellulose (TAC) film (trade name "DSR3-LR", manufactured by Dainippon Printing Co., Ltd., total thickness 45 μm, anti-glare / anti-reflection treatment) so that no bubbles would enter. In this way, a laminate having a structure of [TAC film / binder adhesive layer / release liner] was produced.

[0103] <PET film / ultraviolet curable adhesive layer / radiation non-curable adhesive layer> (ultraviolet curable adhesive layer) 189.77 parts by mass of butyl acrylate (BA), 38.04 parts by mass of cyclohexyl acrylate (CHA), 85.93 parts by mass of 2-hydroxyethyl acrylate (HEA), 0.94 parts by mass of 2,2'-azobisisobutyronitrile as a polymerization initiator, and 379.31 parts by mass of methyl ethyl ketone as a polymerization solvent were placed in a 1L round-bottom separable flask, a separable cover, a separating funnel, a thermometer, a nitrogen inlet tube, a Liebig condenser, a vacuum seal, a stirring rod, and a stirring blade. The mixture was stirred and substituted with nitrogen at room temperature for 6 hours. After that, the mixture was polymerized by holding at 65°C for 4 hours and at 75°C for 2 hours under nitrogen flow and stirring to obtain a resin solution. The resin solution obtained was then cooled to room temperature. After that, 57.43 parts by mass of 2-isocyanatoethyl methacrylate (product name "Kalends MOI", manufactured by Showa Denko K.K.) was added to the resin solution as a compound having a polymerizable carbon-carbon double bond. Furthermore, 0.29 parts by mass of dibutyltin(IV) dilaurate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added, and the mixture was stirred at 50°C for 24 hours under an air atmosphere to obtain a base polymer. 100 parts by mass of the solid content of the obtained base polymer was mixed with 1.5 parts by mass of an isocyanate compound (product name "Coronate L", manufactured by Tosoh Corporation, solid content 75% by mass) and 1 part by mass of 2,2-dimethoxy-1,2-diphenyl-1-one (product name "omnirad 651", manufactured by IGM Resins Italia Srl). The solid content was adjusted to 20 to 40% by mass using toluene as a dilution solvent, to obtain an adhesive solution (1).

[0104] This adhesive solution (1) was applied onto the treated surface of a PET film (product name "T912E75 (UE80-)", manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) so that the thickness after drying would be 112.5 μm, and the film was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form an ultraviolet-curable adhesive layer (1). On the other hand, the adhesive solution (1) obtained above was applied onto the release-treated surface of a release liner (product name "MRF38", manufactured by Mitsubishi Chemical Corporation) so that the thickness after drying would be 112.5 μm, and the film was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form an ultraviolet-curable adhesive layer (2).

[0105] Then, the adhesive layer surfaces of the ultraviolet-curable adhesive layer (1) formed on the PET film and the ultraviolet-curable adhesive layer (2) formed on the release liner were attached to each other using a hand roller while avoiding the inclusion of air bubbles, to form one ultraviolet-curable adhesive layer. The release liner was then peeled off. In this way, a laminate having a configuration of [PET film / ultraviolet-curable adhesive layer] was produced.

[0106] (Radiation non-curable adhesive layer) 189.77 parts by mass of butyl acrylate (BA), 38.04 parts by mass of cyclohexyl acrylate (CHA), 85.93 parts by mass of 2-hydroxyethyl acrylate (HEA), 0.94 parts by mass of 2,2'-azobisisobutyronitrile as a polymerization initiator, and 379.31 parts by mass of methyl ethyl ketone as a polymerization solvent were placed in a 1L round-bottom separable flask, a separable cover, a separating funnel, a thermometer, a nitrogen inlet tube, a Liebig condenser, a vacuum seal, a stirring rod, and a stirring blade. The mixture was stirred and substituted with nitrogen at room temperature for 6 hours. After that, the mixture was polymerized by holding at 65°C for 4 hours and at 75°C for 2 hours under nitrogen flow and stirring to obtain a resin solution. The obtained resin solution was mixed with 1.5 parts by mass of an isocyanate compound (product name "Coronate L", manufactured by Tosoh Corporation, solid content 75% by mass) per 100 parts by mass of the solid content of the base polymer. The solid content was adjusted to 20 to 40% by mass using toluene as a dilution solvent to obtain an adhesive solution (2).

[0107] This pressure-sensitive adhesive solution (2) was applied onto the release-treated surface of a release liner (trade name "MRF38", manufactured by Mitsubishi Chemical Corporation) so that the thickness after drying would be 25 μm, and was heat-dried at 125°C for 2 minutes under normal pressure to form a radiation non-curable pressure-sensitive adhesive layer.

[0108] (PET film / UV curable pressure-sensitive adhesive layer / radiation non-curable pressure-sensitive adhesive layer) The above radiation non-curable pressure-sensitive adhesive layer was laminated onto the UV curable pressure-sensitive adhesive layer surface of a laminate having a [PET film / UV curable pressure-sensitive adhesive layer] structure using a hand roller so that no bubbles would enter. In this way, a laminate having a [PET film / UV curable pressure-sensitive adhesive layer / radiation non-curable pressure-sensitive adhesive layer / release liner] structure was produced.

[0109] <Sheet for encapsulating optical semiconductor element> The release liner was peeled off from a laminate having a [TAC film / binder pressure-sensitive adhesive layer / release liner] structure, and the exposed binder pressure-sensitive adhesive layer surface was laminated onto the PET film surface of a laminate having a [PET film / UV curable pressure-sensitive adhesive layer / radiation non-curable pressure-sensitive adhesive layer / release liner] structure using a hand roller so that no bubbles would enter. Thereafter, aging was performed at 50°C for 48 hours to produce a sheet for encapsulating an optical semiconductor element of Example 1 having a layer structure of [TAC film / binder pressure-sensitive adhesive layer / PET film / UV curable pressure-sensitive adhesive layer / radiation non-curable pressure-sensitive adhesive layer / release liner].

[0110] Example 2 A sheet for encapsulating an optical semiconductor element of Example 2 was produced in the same manner as in Example 1, except that the thickness of the UV curable pressure-sensitive adhesive layer (1) was 100 μm, the thickness of the UV curable pressure-sensitive adhesive layer (2) was 100 μm (total thickness of the UV curable pressure-sensitive adhesive layer: 200 μm), and the thickness of the radiation non-curable pressure-sensitive adhesive layer was 50 μm.

[0111] Example 3 (PET film / UV curable pressure-sensitive adhesive layer / radiation non-curable pressure-sensitive adhesive layer) (UV curable adhesive layer) The adhesive solution (1) prepared in Example 1 was applied onto the treated surface of a PET film (product name "T912E75 (UE80-)", manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) so that the thickness after drying would be 125 μm, and the applied solution was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form an ultraviolet-curable adhesive layer.

[0112] (Radiation non-curable adhesive layer) The adhesive solution (2) prepared in Example 1 was applied onto the release-treated surface of a release liner (product name "MRF38", manufactured by Mitsubishi Chemical Corporation) so that the thickness after drying would be 125 μm, and the applied solution was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form a non-radiation-curable adhesive layer.

[0113] <Optical semiconductor element encapsulation sheet> An optical semiconductor element encapsulation sheet of Example 3 was produced in the same manner as in Example 1, except that the non-radiation-curable pressure-sensitive adhesive layer and the ultraviolet-curable pressure-sensitive adhesive layer obtained above were used.

[0114] Example 4 The adhesive solution (1) prepared in Example 1 was applied to the treated surface of a PET film (product name "T912E75 (UE80-)", manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) so that the thickness after drying would be 125 μm, and the film was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form an ultraviolet-curable adhesive layer (1). On the other hand, the adhesive solution (1) prepared in Example 1 was applied to the release-treated surface of a release liner (product name "MRF38", manufactured by Mitsubishi Chemical Corporation) so that the thickness after drying would be 125 μm, and the film was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form an ultraviolet-curable adhesive layer (2). Then, three layers of the above-mentioned ultraviolet-curable pressure-sensitive adhesive layer (2) prepared separately were laminated on the above-mentioned ultraviolet-curable pressure-sensitive adhesive layer (1) to prepare an ultraviolet-curable pressure-sensitive adhesive layer having a total thickness of 500 μm.

[0115] The adhesive solution (2) prepared in Example 1 was applied onto the release-treated surface of a release liner (product name "MRF38", manufactured by Mitsubishi Chemical Corporation) so that the thickness after drying would be 5 μm, and the applied solution was dried by heating at 125° C. for 2 minutes under normal pressure to form a non-radiation-curable adhesive layer.

[0116] An optical semiconductor element encapsulation sheet of Example 4 was produced in the same manner as in Example 1, except that the non-radiation-curable pressure-sensitive adhesive layer and the ultraviolet-curable pressure-sensitive adhesive layer obtained above were used.

[0117] Example 5 The adhesive solution (1) prepared in Example 1 was applied onto the treated surface of a PET film (product name "T912E75 (UE80-)", manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) so that the thickness after drying would be 25 μm, and the applied solution was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 2 minutes to form an ultraviolet-curable adhesive layer.

[0118] The adhesive solution (2) prepared in Example 1 was applied onto the release-treated surface of a release liner (product name "MRF38", manufactured by Mitsubishi Chemical Corporation) so that the thickness after drying would be 112.5 μm, and the applied solution was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form a non-radiation-curable adhesive layer (1).

[0119] Then, the adhesive layer surfaces of the ultraviolet-curable adhesive layer formed on the PET film and the non-radiation-curable adhesive layer (1) formed on the release liner were attached to each other using a hand roller so as to avoid air bubbles, and then the release liner was peeled off. In this way, a laminate having a configuration of [PET film / ultraviolet-curable adhesive layer / non-radiation-curable adhesive layer (1)] was produced.

[0120] On the other hand, the adhesive solution (2) prepared in Example 1 was applied onto the release-treated surface of a release liner (product name "MRF38", manufactured by Mitsubishi Chemical Corporation) so as to give a thickness after drying of 112.5 μm, and heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form a non-radiation-curable adhesive layer (2).

[0121] Then, the adhesive layer surfaces of the radiation non-curable adhesive layer (1) in the laminate having the configuration of [PET film / ultraviolet ray curable adhesive layer / non-radiation curable adhesive layer (1)] and the radiation non-curable adhesive layer (2) formed on the release liner were bonded together using a hand roller so as to avoid the inclusion of air bubbles, thereby forming one non-radiation curable adhesive layer. In this way, a laminate having the configuration of [PET film / ultraviolet ray curable adhesive layer / non-radiation curable adhesive layer / release liner] was produced.

[0122] The release liner was peeled off from the laminate having the structure of [TAC film / binder adhesive layer / release liner] prepared in Example 1, and the exposed binder adhesive layer surface was attached to the PET film surface of the laminate having the structure of [PET film / ultraviolet ray curable adhesive layer / non-radiation curable adhesive layer / release liner] using a hand roller so as not to trap air bubbles. Then, aging was performed at 50°C for 48 hours to prepare a sheet for encapsulating optical semiconductor elements of Example 5 having a layer structure of [TAC film / binder adhesive layer / PET film / ultraviolet ray curable adhesive layer / non-radiation curable adhesive layer / release liner].

[0123] Comparative Example 1 The adhesive solution (2) prepared in Example 1 was applied onto the treated surface of a PET film (product name "T912E75(UE80-)", manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) to a thickness of 125 μm after drying, and heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form a non-radiation-curable adhesive layer (1). On the other hand, the adhesive solution (2) prepared in Example 1 was applied onto the release-treated surface of a release liner (product name "MRF38", manufactured by Mitsubishi Chemical Corporation) to a thickness of 125 μm after drying, and heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form a non-radiation-curable adhesive layer (2).

[0124] The adhesive layer surfaces of the non-radiation-curable adhesive layer (1) formed on the PET film and the non-radiation-curable adhesive layer (2) formed on the release liner were then bonded together using a hand roller while avoiding the formation of air bubbles, to form one non-radiation-curable adhesive layer. In this manner, a laminate having a configuration of [PET film / non-radiation-curable adhesive layer / release liner] was produced.

[0125] The release liner was peeled off from the laminate having the structure of [TAC film / binder adhesive layer / release liner] prepared in Example 1, and the exposed binder adhesive layer surface was attached to the PET film surface of a laminate having the structure of [PET film / non-radiation curable adhesive layer / release liner] using a hand roller so as to avoid air bubbles. Then, aging was performed at 50°C for 48 hours to prepare a sheet for encapsulating optical semiconductor elements of Comparative Example 1 having a layer structure of [TAC film / binder adhesive layer / PET film / non-radiation curable adhesive layer / release liner].

[0126] Comparative Example 2 The adhesive solution (1) prepared in Example 1 was applied to the treated surface of a PET film (product name "T912E75 (UE80-)", manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) so that the thickness after drying would be 125 μm, and the film was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form an ultraviolet-curable adhesive layer (1). On the other hand, the adhesive solution (1) prepared in Example 1 was applied to the release-treated surface of a release liner (product name "MRF38", manufactured by Mitsubishi Chemical Corporation) so that the thickness after drying would be 125 μm, and the film was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form an ultraviolet-curable adhesive layer (2).

[0127] Then, the adhesive layer surfaces of the ultraviolet-curable adhesive layer (1) formed on the PET film and the ultraviolet-curable adhesive layer (2) formed on the release liner were bonded together using a hand roller while avoiding the inclusion of air bubbles, to form one ultraviolet-curable adhesive layer. In this way, a laminate having a structure of [PET film / ultraviolet-curable adhesive layer / release liner] was produced.

[0128] The release liner was peeled off from the laminate having the structure of [TAC film / binder adhesive layer / release liner] prepared in Example 1, and the exposed binder adhesive layer surface was attached to the PET film surface of the laminate having the structure of [PET film / ultraviolet curable adhesive layer / release liner] using a hand roller so as not to trap air bubbles. Then, aging was performed at 50°C for 48 hours to prepare a sheet for encapsulating optical semiconductor elements of Comparative Example 2 having a layer structure of [TAC film / binder adhesive layer / PET film / ultraviolet curable adhesive layer / release liner].

[0129] Comparative Example 3 The adhesive solution (2) prepared in Example 1 was applied onto the treated surface of a PET film (product name "T912E75(UE80-)", manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) so as to give a dried thickness of 25 μm, and the applied film was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 2 minutes to form a non-radiation curable adhesive layer.

[0130] The adhesive solution (1) prepared in Example 1 was applied onto the release-treated surface of a release liner (product name "MRF38", manufactured by Mitsubishi Chemical Corporation) so that the thickness after drying would be 112.5 μm, and the applied solution was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form an ultraviolet-curable adhesive layer (1).

[0131] Then, the adhesive layer surfaces of the non-radiation curable adhesive layer formed on the PET film and the ultraviolet-curable adhesive layer (1) formed on the release liner were attached to each other using a hand roller so as to avoid air bubbles, and then the release liner was peeled off. In this way, a laminate having a structure of [PET film / non-radiation curable adhesive layer / ultraviolet-curable adhesive layer (1)] was produced.

[0132] On the other hand, the adhesive solution (1) prepared in Example 1 was applied onto the release-treated surface of a release liner (product name "MRF38", manufactured by Mitsubishi Chemical Corporation) so that the thickness after drying would be 112.5 μm, and the applied solution was heated and dried at normal pressure at 50° C. for 1 minute and at 125° C. for 5 minutes to form an ultraviolet-curable adhesive layer (2).

[0133] Then, the adhesive layer surfaces of the ultraviolet-curable adhesive layer (1) in the laminate having the configuration of [PET film / non-radiation-curable adhesive layer / ultraviolet-curable adhesive layer (1)] and the ultraviolet-curable adhesive layer (2) formed on the release liner were bonded together using a hand roller so as to avoid air bubbles, forming one ultraviolet-curable adhesive layer. In this way, a laminate having the configuration of [PET film / non-radiation-curable adhesive layer / ultraviolet-curable adhesive layer / release liner] was produced.

[0134] The release liner was peeled off from the laminate having the structure of [TAC film / binder adhesive layer / release liner] prepared in Example 1, and the exposed binder adhesive layer surface was attached to the PET film surface of the laminate having the structure of [PET film / non-radiation curable adhesive layer / ultraviolet ray curable adhesive layer / release liner] using a hand roller so as not to trap air bubbles. Then, aging was performed at 50°C for 48 hours to prepare a sheet for encapsulating optical semiconductor elements of Comparative Example 3 having a layer structure of [TAC film / binder adhesive layer / PET film / non-radiation curable adhesive layer / ultraviolet ray curable adhesive layer / release liner].

[0135] <Evaluation> The ultraviolet-curable pressure-sensitive adhesive layers and the sheets for encapsulating optical semiconductor elements obtained in the examples and comparative examples were evaluated as follows. The results are shown in the table below.

[0136] (1) Hardness measured by nanoindentation The optical semiconductor element encapsulation sheets obtained in each of the examples and comparative examples were irradiated with ultraviolet light from the TAC film side under the following ultraviolet irradiation conditions to cure the ultraviolet curable adhesive layer. After that, the sheets were frozen at -40°C to -30°C for 10 to 15 minutes, and then cut in the thickness direction using an ultramicrotome under the frozen conditions to expose the cross section of the cured ultraviolet curable adhesive layer. Then, the optical semiconductor element encapsulation sheet with the exposed cross section was fixed to a metal stage attached to the device by solidifying Pentel correction fluid (product number "XEZL1-W"), and then a polyimide film was attached to the window of the device to block light, and evaluation was performed. Using a nanoindenter (product name "TriboIndenter", manufactured by HYSITRON Inc.), nanoindentation measurement was performed on the surface of the cured ultraviolet curable adhesive layer under the following nanoindentation measurement conditions. The obtained hardness is shown in Table 1. <Ultraviolet irradiation conditions> Ultraviolet irradiation device: Product name "UM810", manufactured by Nitto Seiki Co., Ltd. Light source: High pressure mercury lamp Irradiation intensity: 50mW / cm 2 (Measuring equipment: Product name "Ultraviolet Illuminance Meter UT-101", manufactured by Ushio Inc.) Irradiation time: 100 seconds Accumulated light output: 5000mJ / cm 2 <Nanoindentation measurement conditions> Indenter used: Berkovich (triangular pyramid type) Measurement method: Single indentation measurement Measurement temperature: 23℃ Press depth setting: 3.0μm Load speed: 500nm / s Unloading speed: 500nm / s

[0137] (2) Dicing evaluation For the optical semiconductor element encapsulation sheets obtained in the examples and comparative examples, the release liner was peeled off and the entire exposed adhesive layer surface was attached to the pattern surface of a substrate (product name "Lead-free universal substrate ICB93SGPBF", manufactured by Sanhayato Co., Ltd.) with a hand roller to prepare a test sample. The adhesive layer area of ​​the optical semiconductor element encapsulation sheet is larger than the area of ​​the substrate to be attached. The attachment was performed in an environment of a temperature of 22°C and a humidity of 50%, while preventing the inclusion of air bubbles. Thereafter, the above test sample was irradiated with ultraviolet light from the TAC film side under the following ultraviolet light irradiation conditions (1) to cure the ultraviolet-curable adhesive layer. The test sample using the optical semiconductor element encapsulation sheet of Comparative Example 1, which does not have an ultraviolet-curable adhesive layer, was not irradiated with ultraviolet light. <Ultraviolet irradiation conditions (1)> Ultraviolet irradiation device: Product name "UM810", manufactured by Nitto Seiki Co., Ltd. Light source: High pressure mercury lamp Irradiation intensity: 50mW / cm 2 (Measuring equipment: Product name "Ultraviolet Illuminance Meter UT-101", manufactured by Ushio Inc.) Irradiation time: 100 seconds Accumulated light output: 5000mJ / cm 2

[0138] After the ultraviolet irradiation, a dicing tape (product name "NBD-5172K", manufactured by Nitto Denko Corporation) was attached to the surface of the substrate on the side of the test sample on which the optical semiconductor element encapsulation sheet was not attached. A dicing ring for dicing was attached to the adhesive surface of the dicing tape. After attachment, the sample was left for 30 minutes in a light-shielded environment at a temperature of 22°C. Then, the laminate of the test sample and the dicing tape was subjected to blade dicing at a position 5 mm inward from the side edge of the substrate under the following dicing conditions. <Dicing conditions> Dicing equipment: Product name "DFD-6450", manufactured by Disco Corporation Cutting method: Single cut Dicing speed: 30mm / sec Dicing blade: Product name "P1A861 SDC400N75BR597", manufactured by Disco Corporation Dicing blade rotation speed: 30,000 rpm Blade height: 85μm Water amount: 1.5L / min Dicing interval: 10mm Distance of one dicing: Full length of test sample

[0139] The blade used for dicing was one that had been dress diced using the following method. A dicing ring and a board (product name "DRESSER BOARD BGCA0172", manufactured by Disco Corporation) were attached to the adhesive layer of a dicing tape (product name "NBD-7163K", manufactured by Nitto Denko Corporation) to prepare a workpiece for processing. The workpiece was then diced under the following dress dicing conditions to obtain a blade for the blade dicing. <Dress dicing conditions> Dicing equipment: Product name "DFD-6450", manufactured by Disco Corporation Cutting method: Single cut Dicing speed: 55mm / sec Dicing blade: Product name "P1A861 SDC400N75BR597" (new), manufactured by Disco Corporation Dicing blade rotation speed: 35,000 rpm Blade height: 500μm Water amount: 1.5L / min Distance per dicing: Total length of board Dicing interval: 1mm increments Dicing times: 100 times

[0140] After the blade dicing, ultraviolet light was irradiated from the dicing tape base material side under the ultraviolet light irradiation conditions (2) described below to reduce the peel strength of the dicing tape to the substrate. <Ultraviolet irradiation conditions (2)> Ultraviolet irradiation device: Product name "UM810", manufactured by Nitto Seiki Co., Ltd. Light source: High pressure mercury lamp Irradiation intensity: 50mW / cm 2 (Measuring equipment: Product name "Ultraviolet Illuminance Meter UT-101", manufactured by Ushio Inc.) Irradiation time: 10 seconds Accumulated light output: 500mJ / cm 2

[0141] The laminate of the test sample and the substrate, which had been cut into strips by blade dicing, was then peeled off from the dicing tape. Test samples that were confirmed to have peeled off from the substrate during dicing were rated as "B," and those that did not show any peeling were rated as "A."

[0142] (3) Thread drawing evaluation Two laminates of the test sample and the substrate cut into strips in the above dicing evaluation were peeled off from the dicing tape. Next, the two laminates were bonded together with the cut surfaces exposed by dicing, and left in that state for 24 hours in an environment at a temperature of 50°C. The two bonded strips were then removed and left in an environment at a temperature of 22°C and humidity of 50% for 3 hours. Then, an attempt was made to peel the bonded cut surfaces off by hand, and those that could not be peeled off or could be peeled off but the adhesive layer was noticeably stringy were rated as "D", those that could be peeled off but the adhesive layer was slightly stringy were rated as "C", those that required force to peel off but could be peeled off without the adhesive layer being stringy were rated as "B", and those that did not require any particular force to peel off and could be peeled off without the adhesive layer being stringy were rated as "A".

[0143] [Table 1]

[0144] As shown in Table 1, the optical semiconductor element encapsulation sheet (Example) of the present invention had good results in the dicing evaluation, and was evaluated as having excellent adhesion of the sheet to the optical semiconductor element and the substrate, and excellent encapsulation of the optical semiconductor element. In addition, the stringiness evaluation had good results, and it was evaluated that the adhesion of the encapsulation side surface was low, and that when adjacent optical semiconductor devices were pulled apart, damage to the sheet and adhesion of the sheets of adjacent optical semiconductor devices were unlikely to occur.

[0145] On the other hand, when there was no ultraviolet-curable adhesive layer (Comparative Example 1), the results of the stringiness evaluation were poor. Also, when there was no radiation-non-curable adhesive layer (Comparative Example 2) and when the layer located on the surface on the optical semiconductor element side was an ultraviolet-curable adhesive layer (Comparative Example 3), the results of the dicing evaluation were poor, and the sealing ability of the optical semiconductor element was evaluated to be poor. [Explanation of symbols]

[0146] 1. Optical semiconductor element encapsulation sheet 1' Cured sheet for sealing optical semiconductor elements 2 Base material part 21 Optical Film 22 Adhesive layer 23 Plastic Film 3 Sealing part 31 Radiation curable resin layer 31' Cured sealing layer 32 Radiation non-curable adhesive layer 4 Release Liner 5 Substrate 6 Optical semiconductor devices 10,20 Optical semiconductor device

Claims

1. A sheet for encapsulating one or more optical semiconductor elements disposed on a substrate, comprising: a substrate and a seal provided on one surface of the substrate for sealing the optical semiconductor element; a stopper portion; The sealing portion is a radiation-resistant material that is located on the surface of the optical semiconductor element when the optical semiconductor element is sealed. A curable adhesive layer and a radiation curable resin layer laminated on the non-radiation curable adhesive layer. Has the substrate, the radiation curable resin layer, and the non-radiation curable pressure-sensitive adhesive layer are laminated in this order; the radiation is at least one selected from the group consisting of an electron beam, an ultraviolet ray, an α-ray, a β-ray, a γ-ray, and an X-ray; The non-radiation-curable pressure-sensitive adhesive layer is formed of a pressure-sensitive adhesive,

2. The radiation curable resin layer is thicker than the non-radiation curable adhesive layer according to claim 1 . Sheet for sealing optical semiconductor elements.

3. 3. The optical semiconductor element encapsulation shield according to claim 1, wherein the encapsulating portion includes a layer containing a colorant. Quote.

4. 4. The display device according to claim 1, further comprising a layer having anti-glare and / or anti-reflection properties.

3. The sheet for encapsulating an optical semiconductor element according to claim 1.

5. The present invention provides a layer mainly composed of a polyester resin and / or a polyimide resin. Item 5. The sheet for encapsulating an optical semiconductor element according to any one of items 1 to 4.

6. Nanoindentation at a temperature of 23° C. on a cross section of the radiation curable resin layer after curing The optical fiber according to any one of claims 1 to 5, wherein the hardness measured by the flexural modulus test is 1.4 MPa or more. Sheet for sealing semiconductor elements.

7. 7. The sheet for encapsulating an optical semiconductor element according to claim 1, wherein the non-radiation-curable pressure-sensitive adhesive layer and the radiation-curable resin layer are directly laminated together without any other layer therebetween.

8. A substrate, an optical semiconductor element disposed on the substrate, and a method for sealing the optical semiconductor element, comprising: Item 8. The radiation curable resin layer of the optical semiconductor element encapsulation sheet according to any one of items 1 to 7. and a cured product.

9. 9. The optical semiconductor device according to claim 8, which is a backlight for a liquid crystal display.

10. An image display device comprising the backlight according to claim 9 and a display panel.

11. 9. The optical semiconductor device according to claim 8, which is a self-luminous display device.

12. An image display device comprising the self-luminous display device according to claim 11.

13. A substrate, an optical semiconductor element disposed on the substrate, and a method for sealing the optical semiconductor element, comprising: Item 8. The radiation curable resin layer of the optical semiconductor element encapsulation sheet according to any one of items 1 to 7. A dicing step of dicing the laminate having the cured product to obtain an optical semiconductor device. The method for manufacturing an optical semiconductor device includes the steps of:

14. Furthermore, the substrate, an optical semiconductor element disposed on the substrate, and a semiconductor device for sealing the optical semiconductor element are provided. and exposing a laminate having the optical semiconductor element encapsulating sheet to radiation to form the radiation. The method according to claim 13, further comprising a radiation exposure step of curing the curable resin layer to obtain the cured product. The present invention relates to a method for manufacturing an optical semiconductor device.

15. The optical semiconductor element encapsulation sheet is attached to the optical semiconductor element provided on the substrate. and then sealing the optical semiconductor element with the sealing part. The method for producing an optical semiconductor device according to claim 14 , further comprising an irradiation step.

16. Furthermore, the plurality of optical semiconductor devices obtained in the dicing step are diced together in such a way that they are in contact with each other in a planar direction. The optical semiconductor device according to any one of claims 13 to 15, further comprising a tiling step of arranging the optical semiconductor device in a manner similar to that of the optical semiconductor device according to claim 13. Manufacturing method of the device.

Citation Information

Patent Citations

  • Micro light-emitting diode display device and manufacturing method thereof

    CN111276505A

  • Cleaner in sewer pipe

    JP1989011685A

  • Glareproofing agent, glareproof film, and production thereof

    JP1998219136A

  • Thermosetting silicone resin composition, and optical semiconductor device and semiconductor package using molded article thereof

    JP2017066390A

  • Adhesive sheet and display body

    JP2017075281A