Heterocyclic compounds or their salts, active materials, electrolytes, and redox flow batteries
Heterocyclic compounds enhance the energy density and cycle characteristics of redox flow batteries by serving as active materials in aqueous electrolytes, addressing resource constraints and safety issues of vanadium-based systems.
Patent Information
- Application Number
- JP2022510520
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-18
- Filing Date
- 2021-03-23
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-03-23
Smart Images

Figure 0007572426000038 
Figure 0007572426000039 
Figure 0007572426000040
Abstract
Description
[Technical field]
[0001] The present invention relates to a heterocyclic compound or a salt thereof. The present invention also relates to an active material containing the heterocyclic compound or a salt thereof, an electrolyte containing the active material, and a redox flow battery including the electrolyte. [Background technology]
[0002] With the increase in installed capacity due to renewable energy, the introduction of large-scale storage batteries is being promoted to stabilize grid power. Redox flow batteries, which are expected to be large-scale storage batteries, have aqueous and non-aqueous electrolytes, but aqueous electrolytes are superior in terms of safety and cost. Therefore, active materials are required to have high solubility in water and an appropriate redox potential to achieve high energy density.
[0003] In addition, vanadium is currently used as the active material in redox flow batteries. However, the use of vanadium is subject to resource constraints, and price fluctuations are an issue (Non-Patent Documents 1, 2). Therefore, it is desirable to use abundant materials as the active material. [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] Jan Winsberg et al., Angew. Chem. Int. Ed. 2017, 56, 686-711 [Non-Patent Document 2] P. Leung et al., Journal of Power Sources 360 (2017) 243-283 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a novel compound, active material, electrolyte, and redox flow battery that enable improvement in the energy density and cycle characteristics of a redox flow battery using an aqueous electrolyte. [Means for solving the problem]
[0006] The heterocyclic compound or a salt thereof according to an embodiment of the present invention is represented by the following formula (1), (2) or (3). [ka] (In the above formula (1), R 1 ~R 8 are each independently a hydrogen atom, an acidic group, an alkoxy group, an alkyl group, an amino group, an amide group, or a group represented by formula (a), and R 1 ~R 8 At least one of the groups is a group represented by formula (a), X 1 is an oxygen atom, a sulfur atom or NY 2 and Y 1 is a group represented by formula (b), Y 2 is a hydrogen atom, an alkyl group, a carbonyl group, a sulfonyl group, or a group represented by formula (b), R 9 and R 10 each independently represents a hydrogen atom or a substituent, Z 1 is an acidic group, n represents an integer from 1 to 7; * a represents a bonding site with formula (1); * b is X in formula (a) 1 represents the binding site with [ka] (In formula (2), X 2 is an oxygen atom, a sulfur atom, or NR 11 and Y 2is the linker, Z 2 is an acidic group, n 1 is an integer from 1 to 6, R 11 is a hydrogen atom or an alkyl group, R 12 are each independently an alkyl group or an acidic group, n 2 is an integer between 0 and 5); [ka] (In formula (3), X 3 is an oxygen atom or a sulfur atom, Y 3 is the linker, Z 3 is an acidic group, n 3 is an integer from 3 to 8, R 13 are each independently an alkyl group or an acidic group, n 4 is an integer between 0 and 5)
[0007] In one embodiment of the present invention, Z in formula (b) 1 is a sulfo group.
[0008] In one embodiment of the present invention, R 1 ~R 8 At least two of these are groups represented by the formula (a).
[0009] In one embodiment of the present invention, R 2 and R 3 is a group represented by the formula (a).
[0010] The active material according to the embodiment of the present invention contains at least one of the above heterocyclic compounds or salts thereof.
[0011] The electrolyte solution according to the embodiment of the present invention contains the above-mentioned active material.
[0012] In one embodiment of the present invention, the electrolyte is an electrolyte for a redox flow battery.
[0013] In one embodiment of the present invention, the content of water contained in the electrolytic solution is 1% by mass or more and 99.99% by mass or less.
[0014] In one embodiment of the present invention, the content of water in the electrolytic solution is 10% by mass or more and 99% by mass or less.
[0015] A redox flow battery according to an embodiment of the present invention includes the above-described electrolyte.
[0016] In one embodiment of the present invention, the redox flow battery further comprises an electrode and a membrane. Effect of the Invention
[0017] According to the present invention, it is possible to realize a novel compound, active material, electrolyte, and redox flow battery that enable improvement in the energy density and cycle characteristics of a redox flow battery using an aqueous electrolyte. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a charge / discharge curve diagram showing the redox flow battery 1 produced in Example 4. [Diagram 2] FIG. 1 is a charge / discharge curve diagram showing the redox flow battery 2 produced in Example 5. [Diagram 3] FIG. 1 is a charge / discharge curve diagram showing the redox flow battery 3 produced in Example 6. [Figure 4] FIG. 1 is a charge / discharge curve diagram showing the redox flow battery 4 produced in Example 9. [Diagram 5] FIG. 13 is a charge / discharge curve diagram showing the redox flow battery 5 produced in Example 12. [Figure 6]FIG. 13 is a charge / discharge curve diagram showing the redox flow battery 6 produced in Example 13. [Figure 7] FIG. 15 is a charge / discharge curve diagram showing the redox flow battery 7 produced in Example 15. [Figure 8] FIG. 2 is a charge / discharge curve diagram showing the redox flow battery 8 produced in Example 22. [Figure 9] FIG. 2 is a charge / discharge curve diagram showing the redox flow battery 9 produced in Example 23. [Figure 10] FIG. 2 is a charge / discharge curve diagram showing the redox flow battery 10 produced in Example 24. [Figure 11] FIG. 2 is a charge / discharge curve diagram showing the redox flow battery 11 produced in Example 25. [Figure 12] FIG. 2 is a charge / discharge curve diagram showing the redox flow battery 12 produced in Example 26. [Figure 13] FIG. 2 is a charge / discharge curve diagram showing the redox flow battery 13 produced in Example 27. [Figure 14] FIG. 2 is a charge / discharge curve diagram showing the redox flow battery 14 produced in Comparative Example 1. [Figure 15] FIG. 1 is a charge / discharge curve diagram showing the redox flow battery 15 produced in Comparative Example 2. [Figure 16] FIG. 11 is a charge / discharge curve diagram showing the redox flow battery 16 produced in Comparative Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The present invention will be described in detail below. In this specification, including the examples, unless otherwise specified, "parts" and "%" are all based on mass. In addition, to avoid complexity, the description of "compound or a salt thereof" may be simply referred to as "compound" for convenience.
[0020] <Heterocyclic compounds> The heterocyclic compound according to the present embodiment is represented by the following formula (1), (2) or (3). That is, the heterocyclic compound is selected from the group consisting of a phenazine-based compound represented by the following formula (1), a naphthoquinone-based compound represented by the following formula (2) and an anthraquinone-based compound represented by the following formula (3). By including such a heterocyclic compound as an active material in an aqueous electrolyte for a redox flow battery, the energy density and cycle characteristics of the redox flow battery can be improved. When these compounds form salts, for example, they may be alkali metal salts such as lithium salts, sodium salts and potassium salts, alkaline earth metal salts such as calcium salts, ammonium salts, ammonium salts such as tetramethylammonium salts, and the like. In addition, when the compound represented by formula (1), formula (2) or formula (3) has a plurality of acidic groups, they may all be free acids, all be salts, or some may be free acids (some may be salts). When a plurality of salts are present in these compounds, the salts may be the same type of salt or different types of salts.
[0021] [ka]
[0022] [ka]
[0023] [ka]
[0024] [Phenazine-based compound represented by formula (1)] In formula (1), R 1 ~R 8 are each independently a hydrogen atom, an acidic group, an alkoxy group, an alkyl group, an amino group, an amide group, or a group represented by formula (a), and R 1 ~R 8 At least one of X in formula (a) is a group represented by formula (a). 1 is an oxygen atom, a sulfur atom or NY2 and Y 1 is a group represented by formula (b). 2 is a hydrogen atom, an alkyl group, a carbonyl group, a sulfonyl group, or a group represented by formula (b). 9 and R 10 each independently represents a hydrogen atom or a substituent; Z 1 is an acidic group, and n is an integer of 1 to 7. * a represents a bonding site with formula (1); * b is X in formula (a) 1 represents the binding site with
[0025] Examples of the acidic group include a sulfo group, a carboxy group, a phosphoric acid group, and a hydroxyl group, and the sulfo group is preferable. These acidic groups may be in the form of a free acid or a salt.
[0026] Examples of the alkoxy group include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, and a t-butoxy group.
[0027] Examples of the amino group include an amino group (-NH2), a methylamino group, a dimethylamino group, an ethylamino group, and a diethylamino group, with an amino group being preferred.
[0028] Examples of the amide group include a formamide group, an acetamide group, a benzamide group, and a pivalamide group, with an acetamide group being preferred.
[0029] Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, and a t-butyl group.
[0030] Examples of the carbonyl group include an acetyl group, a pivaloyl group, and a benzoyl group, with acetyl being preferred.
[0031] Examples of the sulfonyl group include a methanesulfonyl group, a p-toluenesulfonyl group, an o-nitrobenzenesulfonyl group, and a trifluoromethanesulfonyl group.
[0032] The substituent may, for example, be an alkyl group.
[0033] n is preferably 1 to 6, more preferably 1 to 3, further preferably 1 or 2, and particularly preferably 2.
[0034] R in formula (1) 1 ~R 8 Among these, it is preferable that at least two of them are groups represented by the above formula (a), and R 2 and R 3 It is more preferable that Z in formula (b) is a group represented by the above formula (a). 1 is preferably a sulfo group.
[0035] As a specific embodiment of the phenazine compound represented by formula (1), R 2 is a group represented by the above formula (a), and R 3 is a group represented by the above formula (a) or an acidic group, and R 6 is a hydrogen atom, an amide group, an amino group, or an acidic group, and R 1 , R 4 , R 5 , R 7 and R 8 are each a hydrogen atom, and X in formula (a) 1 is an oxygen atom, and R in formula (b) 9 and R 10 It is preferred that each of the groups is a hydrogen atom and n is 2.
[0036] The phenazine compound represented by formula (1) may be used alone or in combination of two or more. When two or more types are used in combination, they can be used in any ratio.
[0037] [Naphthoquinone compound represented by formula (2)] In formula (2), X 2 is an oxygen atom, a sulfur atom, or NR 11 and Y 2 is a linker, Z 2 is an acidic group. 1 is an integer from 1 to 6, and R 11 is a hydrogen atom or an alkyl group. 12 are each independently an alkyl group or an acidic group, and n 2 is an integer from 0 to 5.
[0038] Examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an iso-propyl group, an n-butyl group, a sec-butyl group, a tert-butyl group, and an n-hexyl group. These alkyl groups may further have a substituent such as a hydroxy group, a thiol group, an alkoxy group, an amino group, or a nitrile group.
[0039] The linker is X in formula (2). 2 and Z 2 For example, an alkylene portion, such as "(alkylene-oxygen atom) m -alkylene linking moiety".
[0040] Examples of the alkylene moiety include a methylene moiety (-CH2-), an ethylene moiety (-CH2CH2-), a propylene moiety (-CH2CH2CH2-), a butylene moiety (-CH2CH2CH2CH2-), an isopropylene moiety (-CH(CH3)CH2-), and the like, with a propylene moiety being preferred.
[0041] "(Alkylene-oxygen atom) m Examples of the -alkylene linking moiety (m is an integer of 1 to 5, and the alkylene and alkylene linking moiety can be selected from the examples of the alkylene moiety above) include an ethoxyethyl moiety (-CH2CH2OCH2CH2-), a methoxyethyl moiety (-CH2OCH2CH2-), -CH2CH2O-CH2CH2O-CH2CH2-, and the like.
[0042] Examples of the acidic group include a sulfo group, a carboxy group, a phosphoric acid group, and a hydroxyl group, and the sulfo group and the carboxy group are preferable. These acidic groups may be in the form of a free acid or a salt.
[0043] n 1 is preferably 1 to 4, more preferably 1 or 2, and particularly preferably 2. 1 If is 2 or more, each X 1 , each Y 1 , each Z 1 may be independently the same or different.
[0044] n 2 is preferably 0 to 3, more preferably 0 to 1, and particularly preferably 0. 2 If is 2 or more, each R 12 may be independently the same or different.
[0045] The naphthoquinone compound represented by formula (2) is 2 is a sulfur atom, and Y 2 is the propylene moiety, and Z 2 is an acidic group, and n 1 is 2, and n 2 is preferably 0. That is, in formula (2), it is preferable that the benzene ring in the naphthoquinone skeleton does not have a substituent.
[0046] The naphthoquinone-based compound represented by formula (2) may be used alone or in combination of two or more. When two or more types are used in combination, they can be used in any ratio.
[0047] [Anthraquinone compound represented by formula (3)] In formula (3), X 3 is an oxygen atom or a sulfur atom, and Y 3 is a linker, Z 3 is an acidic group. 3 is an integer from 3 to 8.13 are each independently an alkyl group or an acidic group, and n 4 is an integer of 0 to 5. In formula (3), the linker, the acidic group, and the alkyl group are each the same as defined in formula (2) above.
[0048] X 3 is preferably an oxygen atom, n 3 is preferably 3 to 6. 3 , each Y 3 , each Z 3 may be independently the same or different.
[0049] As the anthraquinone compound represented by formula (3), X 3 is an oxygen atom, and Y 3 is a methylene moiety, a propylene moiety or -CH2CH2O-CH2CH2O-CH2CH2-, and Z 3 is a sulfo group, a carboxy group, or a hydroxyl group, and n 3 is 3, 4 or 6, and n 4 is preferably 0. More specifically, X in formula (3) 3 is an oxygen atom, and Y 3 is the propylene moiety, and Z 3 is a sulfo group, and n 3 is 3, and n 4 is 0, and X is at the 1st, 2nd, and 3rd positions of the anthraquinone skeleton, respectively. 3 Compounds substituted with X in formula (3) 3 is an oxygen atom, and Y 3 is the propylene moiety, and Z 3 is a sulfo group, and n 3 is 6, and n 4 is 0, and X is at the 1st, 2nd, 3rd, 5th, 6th, and 7th positions of the anthraquinone skeleton, respectively. 3 Compounds substituted with X in formula (3) 3 is an oxygen atom, and Y 3 is a methylene moiety, and Z 3 is a carboxy group, and n 3 is 6, and n 4is 0, and X is at the 1st, 2nd, 3rd, 5th, 6th, and 7th positions of the anthraquinone skeleton, respectively. 3 and a compound substituted with X in formula (3). 3 is an oxygen atom, and Y 3 is the propylene moiety, and Z 3 is a sulfo group, and n 3 is 4, and n 4 is 0, and X is at the 1st, 3rd, 5th, and 7th positions of the anthraquinone skeleton, respectively. 3 Preferred are compounds substituted with:
[0050] The anthraquinone compound represented by formula (3) further includes R 13 R 13 is preferably an acidic group, more preferably a hydroxyl group. 4 is n 3 The number of and n 4 The sum of these numbers may be set to 8 or less, preferably 1 to 2, and particularly preferably 2.
[0051] More specifically, X in formula (3) 3 is an oxygen atom, and Y 3 is -CH2CH2O-CH2CH2O-CH2CH2-, and Z 3 is a hydroxyl group, n 3 is 4 and R 13 is a hydroxyl group, n 4 is 0, and X is at the 1st, 3rd, 5th, and 7th positions of the anthraquinone skeleton, respectively. 3 is substituted, and R is substituted at the 2nd and 6th positions, 13 Particularly preferred is a compound substituted with: Such a compound is represented by the following formula (3'):
[0052] [ka]
[0053] The anthraquinone compound represented by formula (3) may be used alone or in combination of two or more. When two or more types are used in combination, they can be used in any ratio.
[0054] <Active material> The active material according to the present embodiment contains at least one heterocyclic compound represented by the above formula (1), (2) or (3) or a salt thereof. By adding such an active material to an aqueous electrolyte for a redox flow battery, the energy density and cycle characteristics of the redox flow battery can be improved. The active material may contain any one of these heterocyclic compounds, or may contain two or more of them.
[0055] The active material is preferably an active material for an aqueous electrolyte, and is particularly preferably used in an electrolyte for a redox flow battery as an active material for an aqueous electrolyte. The active material contained in the electrolyte may be either a positive electrode active material or a negative electrode active material, but is preferably a negative electrode active material.
[0056] <Electrolyte> The electrolyte according to the present embodiment contains the above-mentioned active material. The active material according to the present embodiment is preferably an electrolyte for a redox flow battery, since it enables the energy density and cycle characteristics of a redox flow battery using an aqueous electrolyte to be improved. In the electrolyte, the heterocyclic compounds represented by the above formulas (1), (2) and (3) may be contained alone or in combination of two or more. When two or more active materials are used in combination, they may be mixed in any ratio. The content of the active material contained in the electrolyte is preferably 1% by mass or more and 99% by mass or less, more preferably 3% by mass or more and 70% by mass or less.
[0057] The electrolyte may further contain other compounds in addition to the heterocyclic compounds represented by the above formulas (1), (2) and (3) as long as the effects of the present invention are not impaired.
[0058] The electrolyte may contain water, which may be ion-exchanged water, Millipore water, or the like, and is preferably Millipore water.
[0059] The water content in the electrolytic solution can be set arbitrarily, but is preferably from 1 to 99.9% by mass, more preferably from 10 to 99% by mass, and particularly preferably from 75 to 95% by mass.
[0060] When the electrolyte contains, as an active material, a naphthoquinone-based compound represented by the above formula (2) and / or an anthraquinone-based compound represented by the above formula (3), i.e., a quinone-based compound, it preferably contains a quinone-based compound having a solubility in water of more than 0.07 mol / L, more preferably a solubility in water of 0.1 mol / L or more and 5.0 mol / L or less, even more preferably a solubility in water of 0.15 mol / L or more and 4.0 mol / L or less, and particularly preferably a solubility in water of 0.18 mol / L or more and 3.0 mol / L or less.
[0061] The electrolytic solution may further contain an antifoaming agent. Examples of the antifoaming agent include alcohols such as methanol, ethanol, and propanol, ketones such as acetone and methyl ethyl ketone, polyhydric alcohols such as ethylene glycol, diethylene glycol, propylene glycol, and glycerin, and various commercially available antifoaming agents. Among these, the antifoaming agent is preferably an alcohol, and particularly preferably ethanol. The content of the antifoaming agent contained in the electrolytic solution is not particularly limited, but is preferably 0.1% by mass or more and 10% by mass or less, and more preferably 0.5% by mass or more and 8% by mass or less, based on the amount of water contained in the electrolytic solution.
[0062] <Redox flow battery> The redox flow battery according to the embodiment of the present invention includes the above-mentioned electrolyte. The redox flow battery preferably further includes an electrode and a diaphragm.
[0063] Any material can be selected and used as the electrode as long as it functions as an electrode. For example, it is preferable to use carbon felt, carbon paper, or carbon cloth, and carbon felt is more preferable.
[0064] Any diaphragm can be selected and used as long as it functions as a diaphragm between the electrodes. For example, it is preferable to use an ion exchange membrane, a porous membrane, etc., and it is more preferable to use an ion exchange membrane.
[0065] In the redox flow battery, the same electrolyte solution may be used for the positive electrode and the negative electrode, or different electrolyte solutions may be used. When different electrolyte solutions are used for the positive electrode and the negative electrode, the electrolyte solution according to the present embodiment and a counter electrolyte solution are used in combination.
[0066] In the case of using different electrolytes for the positive electrode and the negative electrode in a redox flow battery, it is preferable to use the electrolyte according to the present embodiment on the negative electrode side and the counterelectrolyte on the positive electrode side, that is, to use the electrolyte according to the present embodiment as the negative electrode electrolyte and the counterelectrolyte as the positive electrode electrolyte.
[0067] Either or both of the electrolyte solution and the counterelectrolyte solution used in the redox flow battery may further contain an electrolyte. Examples of the electrolyte that can be used include lithium hydroxide, sodium hydroxide, potassium hydroxide, lithium carbonate, sodium carbonate, potassium carbonate, ammonium carbonate, sodium hydrogen carbonate, potassium hydrogen carbonate, lithium chloride, sodium chloride, potassium chloride, ammonium chloride, sulfuric acid, acetic acid, formic acid, and hydrochloric acid. Potassium hydroxide or sodium chloride is preferable, and sodium chloride is particularly preferable.
[0068] The counterelectrolyte is not particularly limited as long as it functions as a positive electrode. For example, potassium ferrocyanide, sodium ferrocyanide, ammonium ferrocyanide, ferrocene, TEMPO (2,2,6,6-tetramethylpiperidine-1-oxyl), lithium iodide, sodium iodide, potassium iodide, ammonium iodide, vanadium, etc. can be used. An aqueous solution of potassium ferrocyanide or sodium iodide is preferable, and an aqueous solution of sodium iodide is particularly preferable.
[0069] A redox flow battery includes components such as an electrolyte and an optional counterelectrolyte, electrodes, and a diaphragm, and may further include assembly components such as a container, a sealant, screws, and a bipolar plate, as necessary, in order to configure these components into a battery.
[0070] The electrolyte solution according to the present embodiment and the redox flow battery including the same contain the above-mentioned active material, and therefore have a high energy density and excellent cycle characteristics. In particular, as a redox flow battery using an aqueous electrolyte solution, it is possible to obtain a high energy density, and compared with a non-aqueous electrolyte solution using an organic solvent or the like as a solvent for the electrolyte solution, it is highly safe and has excellent workability and maintainability during the production of the redox flow battery and during replacement of the electrolyte solution. EXAMPLES
[0071] The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto. In addition, unless otherwise specified, room temperature is within the range of 20°C ± 5°C.
[0072] [Synthesis Example 1] 17.6 parts of 1,2-phenylenediamine and 25 parts of 2,5-dihydroxy-1,4-benzoquinone were heated and refluxed for 5 hours and 30 minutes while stirring in 3000 parts of water, then cooled to room temperature and further stirred overnight. A black wet cake was obtained by filtering the suspension obtained and washed with water. The wet cake was dried under reduced pressure at 80°C to obtain 103.2 parts of a wet cake containing 0.163 moles of the compound represented by the following formula (4).
[0073] [ka]
[0074] [Example 1] 51.2 parts of the wet cake containing 0.0808 moles of the compound represented by formula (4) obtained in Synthesis Example 1 and 36.6 parts of 1,8-diazabicyclo[5,4,0]undec-7-ene were dissolved in 410 parts of dimethylformamide, 30.2 parts of 1,3-propane sultone were added, and the mixture was heated to 120°C and stirred for 3 hours. The mixture was then cooled to room temperature, and an excess amount of 25% aqueous sodium hydroxide solution was added and stirred for 30 minutes. The resulting reaction liquid was poured into 3.0 L of acetone, and the precipitated solid was separated by filtration to obtain a wet cake. This was dissolved in 70 parts of water, and 10 parts of 25% aqueous sodium hydroxide solution was added, and the mixture was poured into 1.5 L of ethanol, and the precipitated solid was separated by filtration to obtain a red wet cake. The wet cake was dried under reduced pressure at 80°C to obtain 34.8 parts of the heterocyclic compound of the present invention represented by the following formula (1-1).
[0075] [ka]
[0076] [Synthesis Example 2] 20 parts of 2-nitro-1,4-phenylenediamine was dissolved in 230 parts of toluene to obtain a solution. 9 parts of potassium carbonate was added to this solution, and the temperature was raised to 60°C. While maintaining the temperature at 60°C, 14.7 parts of acetic anhydride was added over 45 minutes and stirred for 1 hour. This solution was cooled to 25°C, and the solid precipitated from the solution was separated by filtration to obtain 35 parts of a wet cake. This wet cake was dried in a hot air dryer at 80°C to obtain 23.9 parts of a compound represented by the following formula (5).
[0077] [ka]
[0078] [Synthesis Example 3] 23.9 parts of the compound represented by formula (5) obtained in Synthesis Example 2 was stirred in 250 parts of ethanol for 30 minutes to obtain a suspension. 0.5 parts of palladium / carbon (Pd10%, about 55% water-wet product) manufactured by Tokyo Chemical Industry Co., Ltd. was added to this suspension, and the mixture was transferred to a pressure-resistant container. Hydrogen gas was injected into the pressure-resistant container, the pressure in the container was adjusted to 0.95 MPa, and the temperature in the container was heated to 65°C. While keeping the temperature in the container at 65°C, hydrogen gas was injected so that the pressure became 0.95 MPa, and the reaction was carried out for 4 hours. After the reaction was completed, the pressure was returned to normal pressure, the reaction liquid was filtered and separated, and ethanol was distilled off under reduced pressure to obtain 19.2 parts of the compound represented by the following formula (6).
[0079] [ka]
[0080] [Synthesis Example 4] The entire amount of the compound represented by formula (6) obtained in Synthesis Example 3 and 19.7 parts of 2,5-dihydroxy-1,4-benzoquinone were heated and refluxed in 400 parts of water, and stirred for a total of 13 hours until the reaction stopped. The resulting suspension was cooled to room temperature, and the precipitated solid was separated by filtration and washed three times with ethanol to obtain a purple wet cake. This wet cake was dried under reduced pressure at 80°C to obtain 44.8 parts of a wet cake containing 0.116 moles of the compound represented by the following formula (7).
[0081] [ka]
[0082] [Example 2] The entire amount of the wet cake containing the compound represented by formula (7) obtained in Synthesis Example 4 and 59.6 parts of 1,8-diazabicyclo[5,4,0]undec-7-ene were dissolved in 530 parts of dimethylformamide, 48.2 parts of 1,3-propane sultone were added, and the mixture was heated to 120°C and stirred for 3 hours. The mixture was then cooled to room temperature, 50 parts of 25% aqueous sodium hydroxide solution was added, and the mixture was stirred for 30 minutes. The resulting reaction liquid was poured into 2.0 L of acetone, and the precipitated solid was separated by filtration to obtain a wet cake. The mixture was dissolved in 300 parts of water, and then poured into 2.0 L of ethanol, and the precipitated solid was separated by filtration to obtain a purple wet cake. The wet cake was dried under reduced pressure at 70°C to obtain 42.9 parts of the heterocyclic compound of the present invention represented by the following formula (1-2).
[0083] [ka]
[0084] [Example 3] 5.6 parts of the heterocyclic compound represented by formula (1-2) obtained in Example 2 was dissolved in 50 parts of 25% aqueous sodium hydroxide solution, heated under reflux for 3 hours while stirring, then cooled to room temperature and stirred overnight. Next, the solvent was removed from the reaction solution obtained by a rotary evaporator to obtain a black solid. This solid was dissolved in 30 parts of water, poured into 800 parts of ethanol, and the precipitated solid was separated by filtration and washed with ethanol. The above-mentioned operation was repeated twice, and finally the obtained wet cake was washed with acetone and dried under reduced pressure at 80°C to obtain 3.7 parts of the heterocyclic compound of the present invention represented by the following formula (1-3).
[0085] [ka]
[0086] [Example 4] The heterocyclic compound represented by formula (1-1) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.1 mol / L to prepare negative electrode electrolyte 1. Meanwhile, sodium ferrocyanide (manufactured by Fujifilm Wako Pure Chemical Industries, content 95% or more) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.2 mol / L to prepare positive electrode electrolyte 1.
[0087] An ion exchange membrane (Sigma-Aldrich Japan, LLC, Nafion (registered trademark) NRE-212) was used as the diaphragm, and carbon felt (Toyobo Co., Ltd., AAF304ZS, 10 mm x 50 mm x 4 mm) was used as the electrode. The carbon felt was inserted into a 10 mm x 50 mm hole in a silicon gasket (thickness 3 mm) and assembled in the order of current collector / electrode / diaphragm / electrode / current collector. The prepared negative electrode electrolyte 1 and positive electrode electrolyte 1 were used as the electrolyte, respectively, to prepare redox flow battery 1.
[0088] The positive electrode electrolyte 1 and the negative electrode electrolyte 1 of the redox flow battery 1 were circulated by a peristaltic pump connected to the outside of the battery through piping, and a test was performed using a multi-electrochemical measurement system (HZ-Pro, manufactured by Hokuto Denko Corporation). The liquid volumes of the positive electrode electrolyte 1 and the negative electrode electrolyte 1 were 20 ml and 6 ml, respectively, and a charge / discharge test was performed at a constant current of 105 mA with an upper limit voltage of 1.6 V and a lower limit voltage of 0.5 V. Figure 1 shows the charge / discharge curves of the redox flow battery 1 up to the fifth cycle. The coulombic efficiency at the fifth cycle was 92%, the voltage efficiency was 89%, and the energy density was 0.90 Wh / L, indicating that good cycle characteristics were obtained.
[0089] [Example 5] The heterocyclic compound represented by formula (1-2) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.1 mol / L to prepare anode electrolyte 2. Meanwhile, sodium ferrocyanide (manufactured by Fujifilm Wako Pure Chemical Industries, content 95% or more) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.2 mol / L to prepare cathode electrolyte 2.
[0090] An ion exchange membrane (Sigma-Aldrich Japan, LLC, Nafion (registered trademark) NRE-212) was used as the diaphragm, and carbon felt (Toyobo Co., Ltd., AAF304ZS, 10 mm x 50 mm x 4 mm) was used as the electrode. The carbon felt was inserted into a 10 mm x 50 mm hole in a silicon gasket (thickness 3 mm) and assembled in the order of current collector / electrode / diaphragm / electrode / current collector. The prepared negative electrode electrolyte 2 and positive electrode electrolyte 2 were used as the electrolyte, respectively, to prepare a redox flow battery 2.
[0091] The positive electrode electrolyte 2 and the negative electrode electrolyte 2 of the redox flow battery 2 were circulated by a peristaltic pump connected to the outside of the battery through piping, and a test was performed using a multi-electrochemical measurement system (HZ-Pro, manufactured by Hokuto Denko Corporation). The liquid volumes of the positive electrode electrolyte 2 and the negative electrode electrolyte 2 were 20 ml and 6 ml, respectively, and a charge / discharge test was performed at a constant current of 105 mA with an upper limit voltage of 1.6 V and a lower limit voltage of 0.5 V. Figure 2 shows the charge / discharge curves of the redox flow battery 2 up to the fifth cycle. The coulombic efficiency at the fifth cycle was 96%, the voltage efficiency was 89%, and the energy density was 1.02 Wh / L, indicating that good cycle characteristics were obtained.
[0092] [Example 6] The heterocyclic compound represented by formula (1-3) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.1 mol / L to prepare anode electrolyte 3. Meanwhile, sodium ferrocyanide (manufactured by Fujifilm Wako Pure Chemical Industries, content 95% or more) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.2 mol / L to prepare cathode electrolyte 3.
[0093] An ion exchange membrane (Sigma-Aldrich Japan, LLC, Nafion (registered trademark) NRE-212) was used as the diaphragm, and carbon felt (Toyobo Co., Ltd., AAF304ZS, 10 mm x 50 mm x 4 mm) was used as the electrode. The carbon felt was inserted into a 10 mm x 50 mm hole in a silicon gasket (thickness 3 mm) and assembled in the order of current collector / electrode / diaphragm / electrode / current collector. The prepared negative electrode electrolyte 3 and positive electrode electrolyte 3 were used as the electrolyte, respectively, to prepare a redox flow battery 3.
[0094] The positive electrode electrolyte 3 and the negative electrode electrolyte 3 of the redox flow battery 3 were circulated by a peristaltic pump connected to the outside of the battery through piping, and a test was performed using a multi-electrochemical measurement system (HZ-Pro, manufactured by Hokuto Denko Corporation). The liquid volumes of the positive electrode electrolyte 3 and the negative electrode electrolyte 3 were 20 ml and 6 ml, respectively, and a charge / discharge test was performed at a constant current of 105 mA with an upper limit voltage of 1.5 V and a lower limit voltage of 0.6 V. Figure 3 shows the charge / discharge curves of the redox flow battery 3 up to the fifth cycle. The coulombic efficiency at the fifth cycle was 98%, the voltage efficiency was 88%, and the energy density was 0.57 Wh / L, indicating that good cycle characteristics were obtained.
[0095] [Table 1]
[0096] [Examples 7-8] 2.5 g of the heterocyclic compound represented by formula (1-1) obtained in Example 1 was weighed into a 10 mL measuring flask and diluted to 10 ml with an aqueous solution containing an antifoaming agent. 6 ml of the obtained electrolyte was transferred to a 20 ml screw-cap bottle (outer diameter 27 mm, height 55 mm, SV-20, manufactured by Nichiden Rika Glass Co., Ltd.). The screw-cap bottle containing the electrolyte was capped and shaken at a pace of 110 times / 30 seconds so that the vertical width was 15 cm for 30 seconds, and after leaving it to stand for 5 minutes, the minimum height of bubbles from the liquid surface on the wall was measured. As shown in Table 2, when no antifoaming agent was added (Example 8), bubbles remained, but the bubbles disappeared when an antifoaming agent was added. In addition, the hyphen "-" in Table 2 indicates that there were no bubbles and the bubble height could not be measured.
[0097] [Table 2]
[0098] [Example 9] The heterocyclic compound represented by formula (1-1) was dissolved in a 6 wt% ethanol aqueous solution to a concentration of 0.5 mol / L to prepare anode electrolyte 4. Meanwhile, sodium iodide (manufactured by Junsei Chemical Co., Ltd., grade 1) was dissolved in a 6 wt% ethanol aqueous solution to a concentration of 2.0 mol / L to prepare cathode electrolyte 4.
[0099] An ion exchange membrane (Sigma-Aldrich Japan, LLC, Nafion (registered trademark) NRE-212) was used as the diaphragm, and carbon felt (Toyobo Co., Ltd., AAF304ZS, 10 mm x 50 mm x 4 mm) was used as the electrode. The carbon felt was inserted into a 10 mm x 50 mm hole in a silicon gasket (thickness 3 mm) and assembled in the order of current collector / electrode / diaphragm / electrode / current collector. The prepared negative electrode electrolyte 4 and positive electrode electrolyte 4 were used as the electrolyte, respectively, to prepare a redox flow battery 4.
[0100] The positive electrode electrolyte 4 and the negative electrode electrolyte 4 of the redox flow battery 4 obtained above were circulated by a peristaltic pump connected to the outside of the battery through piping, and a test was performed using a multi-electrochemical measurement system (HZ-Pro, manufactured by Hokuto Denko Corporation). The amount of the positive electrode electrolyte 4 and the negative electrode electrolyte 4 was 6 ml each, and a charge / discharge test was performed at a constant current of 420 mA with an upper limit voltage of 1.7 V and a lower limit voltage of 0.3 V. Figure 4 shows the charge / discharge curves of the redox flow battery 4 up to the second cycle. The coulombic efficiency in the second cycle was 97%, the voltage efficiency was 66%, and the energy density was 8.92 Wh / L, indicating that good cycle characteristics were obtained.
[0101] [Table 3]
[0102] [Example 10] 2.12 parts of the heterocyclic compound represented by formula (1-1) obtained in Example 1, 8.31 parts of potassium carbonate, and 0.17 parts of potassium iodide were added to 50 parts of dimethylformamide, and 3.51 parts of bromoacetic acid were added dropwise thereto and stirred at room temperature for 20 hours. This reaction solution was poured into 500 mL of acetone, and a red wet cake was obtained by filtration and separation, and washed with a large amount of acetone. This wet cake was dissolved in 40 parts of water, and 2N hydrochloric acid was added dropwise to adjust the pH to 1.0. Again, a black wet cake was obtained by filtration and separation, and washed with water and methanol, and dried under reduced pressure at 80°C to obtain 2.2 parts of the heterocyclic compound of the present invention represented by the following formula (1-4).
[0103] [ka]
[0104] [Synthesis Example 5] 2.52 parts of 3,4-diaminobenzoic acid and 2.56 parts of 2,5-dihydroxy-1,4-benzoquinone were heated and refluxed in 110 parts of water for 3 hours while stirring, then cooled to room temperature and stirred overnight. A red wet cake was obtained from the resulting suspension by filtration and separated, and washed with acetone and water. The wet cake was dried under reduced pressure at 80°C to obtain 4.3 parts of a compound represented by the following formula (8).
[0105] [ka]
[0106] [Example 11] 2.58 parts of the compound represented by formula (8) obtained in Synthesis Example 5 and 4.90 parts of 1,8-diazabicyclo[5,4,0]undec-7-ene were dissolved in 50 parts of dimethylformamide, 3.81 parts of 1,3-propane sultone were added, and the mixture was heated to 120°C and stirred for 1 hour. Then, 2.28 parts of 1,8-diazabicyclo[5,4,0]undec-7-ene and 1.82 parts of 1,3-propane sultone were added and stirred at 120°C for 6 hours. The reaction liquid was cooled to room temperature, 9.6 parts of 25% aqueous sodium hydroxide solution was added dropwise, and the mixture was stirred for 1 hour, and then poured into 500 mL of acetone. A red wet cake was obtained by filtration and separated, and washed with acetone. This wet cake was dissolved in 80 parts of water and poured into 1.0 L of ethanol. The precipitated solid was filtered and washed with ethanol to obtain a brown wet cake. The brown wet cake was further dried under reduced pressure at 80°C to obtain 2.7 parts of the heterocyclic compound of the present invention represented by the following formula (1-5).
[0107] [ka]
[0108] [Example 12] The heterocyclic compound represented by formula (1-4) was dissolved in an aqueous solution (1.0 mol / L) of sodium hydroxide (manufactured by Kokusan Chemical Industries, Ltd., content ≧97.0%) to a concentration of 0.1 mol / L to prepare a negative electrode electrolyte 5. Meanwhile, sodium ferrocyanide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., content ≧95%) was dissolved in an aqueous solution (1.0 mol / L) of sodium hydroxide (manufactured by Kokusan Chemical Industries, content ≧97.0%) to a concentration of 0.2 mol / L to prepare a positive electrode electrolyte 5.
[0109] An ion exchange membrane (Sigma-Aldrich Japan, LLC, Nafion (registered trademark) NRE-212) was used as the diaphragm, and carbon felt (Toyobo Co., Ltd., AAF304ZS, 10 mm x 50 mm x 4 mm) was used as the electrode. The carbon felt was inserted into a 10 mm x 50 mm hole in a silicon gasket (thickness 3 mm) and assembled in the order of current collector / electrode / diaphragm / electrode / current collector. The prepared negative electrode electrolyte 5 and positive electrode electrolyte 5 were used as the electrolyte, respectively, to prepare redox flow battery 5.
[0110] The positive electrode electrolyte 5 and the negative electrode electrolyte 5 of the redox flow battery 5 were circulated by a peristaltic pump connected to the outside of the battery through piping, and a test was performed using a multi-electrochemical measurement system (HZ-Pro, manufactured by Hokuto Denko Corporation). The liquid volumes of the positive electrode electrolyte 5 and the negative electrode electrolyte 5 were 20 ml and 6 ml, respectively, and a charge / discharge test was performed at a constant current of 105 mA with an upper limit voltage of 1.6 V and a lower limit voltage of 0.5 V. Figure 5 shows the charge / discharge curves of the redox flow battery 5 up to the fifth cycle. The coulombic efficiency at the fifth cycle was 81%, the voltage efficiency was 88%, and the energy density was 0.59 Wh / L, indicating that good cycle characteristics were obtained.
[0111] [Example 13] The heterocyclic compound represented by formula (1-5) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.1 mol / L to prepare a negative electrode electrolyte 6. Meanwhile, sodium ferrocyanide (manufactured by Fujifilm Wako Pure Chemical Industries, content 95% or more) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.2 mol / L to prepare a positive electrode electrolyte 6.
[0112] An ion exchange membrane (Sigma-Aldrich Japan, LLC, Nafion (registered trademark) NRE-212) was used as the diaphragm, and carbon felt (Toyobo Co., Ltd., AAF304ZS, 10 mm x 50 mm x 4 mm) was used as the electrode. The carbon felt was inserted into a 10 mm x 50 mm hole in a silicon gasket (thickness 3 mm) and assembled in the order of current collector / electrode / diaphragm / electrode / current collector. The prepared negative electrode electrolyte 6 and positive electrode electrolyte 6 were used as the electrolyte, respectively, to prepare a redox flow battery 6.
[0113] The positive electrode electrolyte 6 and the negative electrode electrolyte 6 of the redox flow battery 6 were circulated by a peristaltic pump connected to the outside of the battery through piping, and a test was performed using a multi-electrochemical measurement system (HZ-Pro, manufactured by Hokuto Denko Corporation). The liquid volumes of the positive electrode electrolyte 6 and the negative electrode electrolyte 6 were 20 ml and 6 ml, respectively, and a charge / discharge test was performed at a constant current of 105 mA with an upper limit voltage of 1.5 V and a lower limit voltage of 0.5 V. Figure 6 shows the charge / discharge curves of the redox flow battery 6 up to the fifth cycle. The coulombic efficiency at the fifth cycle was 89%, the voltage efficiency was 81%, and the energy density was 0.98 Wh / L, indicating that good cycle characteristics were obtained.
[0114] [Table 4]
[0115] [Example 14] 3.03 parts of the compound represented by formula (4) obtained in Synthesis Example 1 and 1.60 parts of 1,8-diazabicyclo[5,4,0]undec-7-ene were dissolved in 100 parts of dimethylformamide, 1.28 parts of 1,3-propane sultone were added, and the mixture was heated to 50°C and stirred for 2 hours. The reaction liquid was cooled to room temperature, 8.0 parts of 25% aqueous sodium hydroxide solution was added dropwise, and the mixture was stirred for 1 hour, and then poured into 500 mL of acetone. A brown wet cake was obtained by filtration and separated, and washed with acetone. This wet cake was dissolved in 50 parts of water, poured into 500 mL of 2-propanol, and the precipitated solid was filtered and washed with ethanol to obtain a brown wet cake, which was dried under reduced pressure at 80°C to obtain 1.4 parts of a brown powder containing the heterocyclic compound of the present invention represented by the following formula (1-6).
[0116] [ka]
[0117] [Example 15] The heterocyclic compound represented by formula (1-6) was dissolved in an aqueous solution (1.0 mol / L) of sodium hydroxide (manufactured by Kokusan Chemical Industries, content ≧97.0%) to a concentration of 0.1 mol / L to prepare a negative electrode electrolyte 7. Meanwhile, sodium ferrocyanide (manufactured by Fujifilm Wako Pure Chemical Industries, content ≧95%) was dissolved in an aqueous solution (1.0 mol / L) of sodium hydroxide (manufactured by Kokusan Chemical Industries, content ≧97.0%) to a concentration of 0.2 mol / L to prepare a positive electrode electrolyte 7.
[0118] An ion exchange membrane (Sigma-Aldrich Japan, LLC, Nafion (registered trademark) NRE-212) was used as the diaphragm, and carbon felt (Toyobo Co., Ltd., AAF304ZS, 10 mm x 50 mm x 4 mm) was used as the electrode. The carbon felt was inserted into a 10 mm x 50 mm hole in a silicon gasket (thickness 3 mm) and assembled in the order of current collector / electrode / diaphragm / electrode / current collector. The above-mentioned negative electrode electrolyte 7 and positive electrode electrolyte 7 were used as the electrolyte, respectively, to prepare redox flow battery 7.
[0119] The positive electrode electrolyte 7 and the negative electrode electrolyte 7 of the redox flow battery 7 were circulated by a peristaltic pump connected to the outside of the battery through piping, and a test was performed using a multi-electrochemical measurement system (HZ-Pro, manufactured by Hokuto Denko Corporation). The liquid volumes of the positive electrode electrolyte 7 and the negative electrode electrolyte 7 were 20 ml and 6 ml, respectively, and a charge / discharge test was performed at a constant current of 105 mA with an upper limit voltage of 1.6 V and a lower limit voltage of 0.5 V. Figure 7 shows the charge / discharge curves up to the fifth cycle. The coulombic efficiency at the fifth cycle was 86%, the voltage efficiency was 91%, and the energy density was 0.83 Wh / L, indicating that good cycle characteristics were obtained.
[0120] [Table 5]
[0121] As shown in Tables 1, 3, 4, and 5 and Figures 1 to 7, the redox flow batteries 1 to 7 prepared in Examples 4 to 6, 9, 12 to 13, and 15 have high average discharge voltages (V) and energy densities, and also have good cycle characteristics. In addition, in Example 7, in which ethanol was added to the electrolyte as a defoaming agent, no air bubbles were generated, and it was confirmed that the electrolyte was easy to handle.
[0122] [Synthesis Example 6] 20 parts of gallic acid was added to 60 parts of sulfuric acid and stirred at 105°C for 3 hours. The reaction solution was cooled to 50°C, poured into 150 parts of ice water, and the resulting suspension was stirred for 1 hour. After stirring, the suspension was filtered and separated to obtain a wet cake. This wet cake was added to 150 parts of cold water, stirred for 30 minutes, and then the suspension was filtered and separated to obtain a wet cake. This wet cake was gradually added to 150 parts of a 5% aqueous sodium hydrogen carbonate solution, stirred for 1 hour, and then the suspension was filtered and separated to obtain a wet cake. This wet cake was dried in a hot air dryer at 80°C to obtain 12.4 parts of a compound represented by the following formula (9).
[0123] [ka]
[0124] [Example 16] 5 parts of the compound represented by formula (9) was added to 45 parts of water and stirred, the pH of the solution was adjusted to 9.5-10.0 with 25% aqueous sodium hydroxide solution, and the temperature was raised to 60°C. 20 parts of propane sultone was added dropwise to the solution over 2 hours, and after the dropwise addition, the solution was stirred at 60°C for 4 hours. During this time, the pH of the solution was maintained at 10.0-10.5 with 25% aqueous sodium hydroxide solution. 500 parts of methanol was added to the obtained reaction solution, and the solution was stirred at 20-25°C for 2 hours. After stirring, the precipitated solid was separated by filtration to obtain 40.8 parts of a wet cake. The wet cake was dried with a hot air dryer at 80°C to obtain 9.2 parts of the heterocyclic compound of the present invention represented by the following formula (3-1).
[0125] [ka]
[0126] [Example 17] The same procedure as in Example 15 was carried out except that 20.5 parts of bromoacetic acid were used instead of 20 parts of propane sultone, and potassium hydroxide was used instead of sodium hydroxide, to obtain 7.9 parts of the heterocyclic compound of the present invention represented by the following formula (3-2).
[0127] [ka]
[0128] [Synthesis Example 7] 10 parts of benzoic acid was added to 60 parts of sulfuric acid, stirred, and heated to 120°C. 13.9 parts of gallic acid was added little by little to the obtained solution and stirred for 7 hours. The reaction solution was cooled to 50°C, added to 150 parts of ice water, and the obtained suspension was stirred for 1 hour. After stirring, the suspension was filtered and separated to obtain a wet cake. This wet cake was added to 150 parts of cold water, stirred for 30 minutes, and then the suspension was filtered and separated to obtain a wet cake. This wet cake was added little by little to 150 parts of 5% aqueous sodium hydrogen carbonate solution, stirred for 1 hour, and the suspension was filtered and separated to obtain a wet cake. This wet cake was dried with a hot air dryer at 80°C to obtain 13.1 parts of a compound represented by the following formula (10).
[0129] [ka]
[0130] [Example 18] 5 parts of the compound represented by formula (10) was added to 45 parts of water and stirred, the pH of the solution was adjusted to 9.5-10.0 with 25% aqueous sodium hydroxide solution, and the temperature was raised to 60°C. 11.9 parts of propane sultone was added dropwise to the solution over 2 hours, and after the dropwise addition, the solution was stirred at 60°C for 4 hours. During this time, the pH of the solution was maintained at 10.0-10.5 with 25% aqueous sodium hydroxide solution. 500 parts of methanol was added to the obtained reaction solution, and the solution was stirred at 20-25°C for 2 hours. The precipitated solid was separated by filtration to obtain 30.7 parts of a wet cake. The wet cake was dried with a hot air dryer at 80°C to obtain 10.8 parts of the heterocyclic compound of the present invention represented by the following formula (3-3).
[0131] [ka]
[0132] [Example 19] 10 parts of 2,3-dichloro-1,4-naphthoquinone was dissolved in 200 parts of N,N-dimethylformamide, and 17 parts of 3-mercapto-1-propanesulfonic acid and 18 parts of potassium carbonate were added, followed by stirring at room temperature for 12 hours. The resulting precipitated solid was separated by filtration and washed with ethanol to obtain a red solid. The resulting solid was dissolved in water, and 1N aqueous hydrochloric acid was added until carbon dioxide gas was no longer generated. Isopropanol was added to the resulting reaction solution, and the precipitated solid was separated by filtration to obtain a wet cake. The wet cake was dried in a hot air dryer at 80°C to obtain 23 parts of the heterocyclic compound of the present invention represented by the following formula (2-1).
[0133] [ka]
[0134] [Synthesis Example 8] 120 parts of concentrated sulfuric acid was heated to 120°C and stirred, and 40 parts of 3,5-dihydroxybenzoic acid was added thereto and stirred for 5 hours. The reaction liquid was cooled to room temperature and added to 500 parts of ice, and the resulting suspension was adjusted to pH 7.5 by adding 25% aqueous sodium hydroxide dropwise while stirring. The resulting suspension was separated by filtration and washed with ice water to obtain a wet cake containing a compound represented by the following formula (11).
[0135] [ka]
[0136] [Example 20] The wet cake containing the compound represented by formula (11) obtained in Synthesis Example 8 was dissolved in 240 mL of water, and 3 / 4 of the total amount was transferred to a 1 L beaker. A 25% aqueous sodium hydroxide solution was added to this aqueous solution to adjust the pH to 10.0-10.2, and the solution was heated to 60°C. A total of 7 equivalents of propane sultone was dropped into the solution, and the solution was stirred at 60°C for 6 hours. During this time, the pH of the solution was maintained at 10.0-10.2 by using a 25% aqueous sodium hydroxide solution. The resulting reaction solution was poured into 800 mL of methanol, and the precipitated solid was separated by filtration to obtain a wet cake. The wet cake was dissolved in 100 parts of a 25% aqueous sodium hydroxide solution, poured into 800 mL of methanol, and the precipitated solid was separated by filtration to obtain a wet cake. This operation was performed twice in total. The resulting wet cake was dissolved in 100 parts of water, adjusted to pH 10.0 using 35% hydrochloric acid, and heated to 60°C. 4 equivalents of propane sultone was added dropwise thereto, and the mixture was stirred at 60° C. for 5 hours. The reaction solution obtained was poured into 800 mL of methanol, and the precipitated solid was separated by filtration to obtain a wet cake. The wet cake was dried in a hot air dryer at 80° C. to obtain 56.6 parts of the heterocyclic compound of the present invention represented by the following formula (3-4).
[0137] [ka]
[0138] [Example 21] 5 parts of the compound represented by the above formula (9), 9.1 parts of potassium carbonate, and 2.7 parts of potassium iodide were added to 45 parts of acetonitrile, and the mixture was stirred and heated to 80°C. 16.4 parts of ethylene glycol mono-2-chloroethyl ether was added dropwise to the solution over 30 minutes, and the mixture was stirred at 80°C for 36 hours after the end of the dropwise addition. The solvent of the obtained reaction solution was distilled off under reduced pressure, 20 parts of water was added, and a brown fraction was separated using SEP-PACK (WATO043345) manufactured by Waters. This aqueous solution was dried with a hot air dryer at 80°C to obtain 8.4 parts of the heterocyclic compound of the present invention represented by the following formula (3-5).
[0139] [ka]
[0140] The solubility in water of each of the heterocyclic compounds (active materials) obtained in Examples 16 to 21 above was calculated from the absorbance. A UV-visible spectrophotometer (UV-1700, manufactured by Shimadzu Corporation) was used to measure the absorbance. A sample solution of known concentration was prepared using a standard buffer solution (Fujifilm Wako Pure Chemical Industries, neutral phosphate pH standard solution, pH 6.86 (25°C)), and the absorbance at the maximum absorption wavelength was measured using the above UV-visible spectrophotometer in the wavelength range of 300 nm to 550 nm. A calibration curve was created from the obtained absorbance and concentration. Subsequently, a saturated solution of the sample was prepared using water, and the solution was diluted using the above standard buffer solution. The absorbance at the maximum absorption wavelength was measured, and the solubility (%) was calculated from the calibration curve. In addition, the density of the solution was set to 1.0 g / cm 3 The solubility (mol / L) was calculated under this assumption. The results are shown in Table 6. In Table 6, the solubility (mol / L) of a conventionally known anthraquinone-based active material is shown for reference.
[0141] [Table 6]
[0142] [Example 22] The heterocyclic compound represented by formula (3-1) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.1 mol / L to prepare a negative electrode electrolyte 8. Meanwhile, sodium iodide (manufactured by Junsei Chemical Co., Ltd., grade 1) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.2 mol / L to prepare a positive electrode electrolyte 8.
[0143] An ion exchange membrane (Sigma-Aldrich Japan, LLC, Nafion (registered trademark) NRE-212) was used as the diaphragm, and carbon felt (Toyobo Co., Ltd., AAF304ZS, 10 mm x 50 mm x 4 mm) was used as the electrode. The carbon felt was inserted into a 10 mm x 50 mm hole in a silicon gasket (thickness 3 mm) and assembled in the order of current collector / electrode / diaphragm / electrode / current collector. The prepared negative electrode electrolyte 8 and positive electrode electrolyte 8 were used as the electrolyte, respectively, to prepare a redox flow battery 8.
[0144] The positive electrode electrolyte 8 and the negative electrode electrolyte 8 of the redox flow battery 8 were circulated by a peristaltic pump connected to the outside of the battery through piping, and a test was performed using a multi-electrochemical measurement system (HZ-Pro, manufactured by Hokuto Denko Corporation). The liquid volumes of the positive electrode electrolyte 7 and the negative electrode electrolyte 7 were 20 ml and 6 ml, respectively, and a charge / discharge test was performed at a constant current of 105 mA with an upper limit voltage of 1.5 V and a lower limit voltage of 0.7 V. Figure 8 shows the charge / discharge curves of the redox flow battery 7 up to the fifth cycle. The coulombic efficiency at the fifth cycle was 84%, the voltage efficiency was 92%, and the energy density was 1.04 Wh / L, indicating that good cycle characteristics were obtained.
[0145] [Example 23] The heterocyclic compound represented by formula (3-2) was dissolved in an aqueous solution (1.0 mol / L) of potassium chloride (manufactured by Junsei Chemical Co., Ltd., special grade) to a concentration of 0.1 mol / L to prepare a negative electrode electrolyte 9. On the other hand, potassium iodide (manufactured by Junsei Chemical Co., Ltd., special grade) was dissolved in an aqueous solution (1.0 mol / L) of potassium chloride (manufactured by Junsei Chemical Co., Ltd., special grade) to a concentration of 0.2 mol / L to prepare a positive electrode electrolyte 9.
[0146] A redox flow battery 9 was produced in the same manner as in Example 22, except that the negative electrode electrolyte 8 and the positive electrode electrolyte 8 in Example 22 were changed to the negative electrode electrolyte 9 and the positive electrode electrolyte 9, respectively. A charge / discharge test was performed using the redox flow battery 9 in the same manner as in Example 22. The amounts of the positive electrode electrolyte 9 and the negative electrode electrolyte 9 were 20 ml and 6 ml, respectively, and a charge / discharge test was performed at a constant current of 105 mA with an upper limit voltage of 1.5 V and a lower limit voltage of 0.7 V. FIG. 9 shows the charge / discharge curves of the redox flow battery 8 up to the fifth cycle. The coulombic efficiency at the fifth cycle was 87%, the voltage efficiency was 88%, and the energy density was 1.08 Wh / L.
[0147] [Example 24] The heterocyclic compound represented by formula (3-3) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.1 mol / L to prepare a negative electrode electrolyte 10. Meanwhile, sodium iodide (manufactured by Junsei Chemical Co., Ltd., grade 1) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.2 mol / L to prepare a positive electrode electrolyte 10.
[0148] A redox flow battery 10 was prepared in the same manner as in Example 22, except that the negative electrode electrolyte 8 and the positive electrode electrolyte 8 in Example 22 were changed to the negative electrode electrolyte 10 and the positive electrode electrolyte 10, respectively. A charge / discharge test was performed using the redox flow battery 10 in the same manner as in Example 22. The amounts of the positive electrode electrolyte 10 and the negative electrode electrolyte 10 were 20 ml and 6 ml, respectively, and the charge / discharge test was performed at a constant current of 105 mA, with an upper limit voltage of 1.4 V and a lower limit voltage of 0.5 V. FIG. 10 shows the charge / discharge curves of the redox flow battery 9 up to the fifth cycle. The coulombic efficiency at the fifth cycle was 84%, the voltage efficiency was 82%, and the energy density was 0.46 Wh / L.
[0149] [Example 25] The heterocyclic compound represented by formula (2-1) was dissolved in an aqueous solution (1.0 mol / L) of potassium hydroxide (manufactured by Junsei Chemical Co., Ltd., special grade) to a concentration of 0.1 mol / L to prepare a negative electrode electrolyte 11. Meanwhile, potassium ferrocyanide (manufactured by Kanto Chemical Co., Ltd., special grade) was dissolved in an aqueous solution (1.0 mol / L) of potassium hydroxide (manufactured by Junsei Chemical Co., Ltd.) to a concentration of 0.2 mol / L to prepare a positive electrode electrolyte 11.
[0150] A redox flow battery 11 was produced in the same manner as in Example 22, except that the negative electrode electrolyte 8 and the positive electrode electrolyte 8 in Example 22 were changed to the negative electrode electrolyte 11 and the positive electrode electrolyte 11, respectively. A charge / discharge test was performed using the redox flow battery 11 in the same manner as in Example 22. The amounts of the positive electrode electrolyte 11 and the negative electrode electrolyte 11 were 20 ml and 6 ml, respectively, and the charge / discharge test was performed at a constant current of 105 mA with an upper limit voltage of 1.3 V and a lower limit voltage of 0.7 V. FIG. 11 shows the charge / discharge curves of the redox flow battery 10 up to the fifth cycle. The coulombic efficiency at the fifth cycle was 88%, the voltage efficiency was 92%, and the energy density was 0.81 Wh / L.
[0151] [Example 26] The heterocyclic compound represented by formula (3-4) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.1 mol / L to prepare a negative electrode electrolyte 12. Meanwhile, sodium iodide (manufactured by Junsei Chemical Co., Ltd., grade 1) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.2 mol / L to prepare a positive electrode electrolyte 12.
[0152] A redox flow battery 12 was produced in the same manner as in Example 22, except that the negative electrode electrolyte 8 and the positive electrode electrolyte 8 in Example 22 were changed to the negative electrode electrolyte 12 and the positive electrode electrolyte 12, respectively. A charge / discharge test was performed using the redox flow battery 12 in the same manner as in Example 22. The amounts of the positive electrode electrolyte 12 and the negative electrode electrolyte 12 were 20 ml and 6 ml, respectively, and the charge / discharge test was performed at a constant current of 105 mA with an upper limit voltage of 1.6 V and a lower limit voltage of 0.5 V. FIG. 12 shows the charge / discharge curves of the redox flow battery 11 up to the fifth cycle. The coulombic efficiency at the fifth cycle was 87%, the voltage efficiency was 91%, and the energy density was 0.85 Wh / L.
[0153] [Example 27] The heterocyclic compound represented by formula (3-5) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.1 mol / L to prepare a negative electrode electrolyte 13. Meanwhile, sodium iodide (manufactured by Junsei Chemical Co., Ltd., grade 1) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.2 mol / L to prepare a positive electrode electrolyte 13.
[0154] A redox flow battery 13 was produced in the same manner as in Example 22, except that the negative electrode electrolyte 8 and the positive electrode electrolyte 8 in Example 22 were changed to the negative electrode electrolyte 13 and the positive electrode electrolyte 13, respectively. A charge / discharge test was performed using the redox flow battery 13 in the same manner as in Example 22. The amounts of the positive electrode electrolyte 13 and the negative electrode electrolyte 13 were 20 ml and 6 ml, respectively, and the charge / discharge test was performed at a constant current of 105 mA with an upper limit voltage of 1.6 V and a lower limit voltage of 0.5 V. FIG. 13 shows the charge / discharge curves of the redox flow battery 12 up to the fifth cycle. The coulombic efficiency at the fifth cycle was 90%, the voltage efficiency was 86%, and the energy density was 0.94 Wh / L.
[0155] [Comparative Example 1] Sodium 9,10-anthraquinone-2-sulfonate was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.1 mol / L to prepare a negative electrode electrolyte 14. Meanwhile, sodium iodide (manufactured by Junsei Chemical Co., Ltd., grade 1) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.2 mol / L to prepare a positive electrode electrolyte 14.
[0156] A redox flow battery 14 was produced in the same manner as in Example 22, except that the negative electrode electrolyte 8 and the positive electrode electrolyte 8 in Example 22 were changed to the negative electrode electrolyte 14 and the positive electrode electrolyte 14, respectively. A charge / discharge test was performed using the redox flow battery 14 in the same manner as in Example 22. The amounts of the positive electrode electrolyte 14 and the negative electrode electrolyte 14 were 20 ml and 6 ml, respectively, and the charge / discharge test was performed at a constant current of 105 mA, with an upper limit voltage of 1.5 V and a lower limit voltage of 0.5 V. FIG. 14 shows the charge / discharge curves of the redox flow battery 14 up to the 5th cycle. In the redox flow battery 14, the active material concentration was insufficient, and good charge / discharge characteristics could not be obtained.
[0157] [Comparative Example 2] Sodium 9,10-anthraquinone-1,5-disulfonate was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.1 mol / L to prepare anode electrolyte 15. Meanwhile, sodium iodide (manufactured by Junsei Chemical Co., Ltd., grade 1) was dissolved in an aqueous solution (1.0 mol / L) of sodium chloride (manufactured by Tokyo Chemical Industry Co., Ltd., purity >99.5%) to a concentration of 0.2 mol / L to prepare cathode electrolyte 15.
[0158] A redox flow battery 15 was prepared in the same manner as in Example 22, except that the negative electrode electrolyte 8 and the positive electrode electrolyte 8 in Example 22 were changed to the negative electrode electrolyte 15 and the positive electrode electrolyte 15, respectively. A charge / discharge test was performed using the redox flow battery 15 in the same manner as in Example 22. The amounts of the positive electrode electrolyte 15 and the negative electrode electrolyte 15 were 20 ml and 6 ml, respectively, and a charge / discharge test was performed at a constant current of 105 mA, with an upper limit voltage of 1.5 V and a lower limit voltage of 0.5 V. FIG. 15 shows the charge / discharge curves of the redox flow battery 15 up to the fifth cycle. The coulombic efficiency at the fifth cycle was 71%, the voltage efficiency was 76%, and the energy density was 0.01 Wh / L. The redox flow battery 15 had inferior cycle characteristics and energy density compared to the redox flow batteries prepared in other examples.
[0159] [Comparative Example 3] Potassium 9,10-anthraquinone-1,8-disulfonate was dissolved in an aqueous solution (1.0 mol / L) of potassium chloride (manufactured by Junsei Chemical Co., Ltd., special grade) to a concentration of 0.1 mol / L to prepare a negative electrode electrolyte 16. On the other hand, potassium iodide (manufactured by Junsei Chemical Co., Ltd., special grade) was dissolved in an aqueous solution (1.0 mol / L) of potassium chloride (manufactured by Junsei Chemical Co., Ltd., special grade) to a concentration of 0.2 mol / L to prepare a positive electrode electrolyte 16.
[0160] A redox flow battery 16 was produced in the same manner as in Example 22, except that the negative electrode electrolyte 8 and the positive electrode electrolyte 8 in Example 22 were changed to the negative electrode electrolyte 16 and the positive electrode electrolyte 16, respectively. A charge / discharge test was performed using the redox flow battery 16 in the same manner as in Example 22. The amounts of the positive electrode electrolyte 16 and the negative electrode electrolyte 16 were 20 ml and 6 ml, respectively, and the charge / discharge test was performed at a constant current of 105 mA, with an upper limit voltage of 1.5 V and a lower limit voltage of 0.7 V. FIG. 16 shows the charge / discharge curves of the redox flow battery 16 up to the 5th cycle. In the redox flow battery 16, the active material concentration was insufficient, and good charge / discharge characteristics could not be obtained.
[0161] [Table 7]
[0162] 8 to 13, it is found that the redox flow batteries 8 to 13 prepared in Examples 22 to 27 have high average discharge voltages (V) and energy densities, and also have good cycle characteristics. In Table 7, "N / A" indicates that the measured value was not available. [Industrial Applicability]
[0163] The active material containing the heterocyclic compound of the present invention, the electrolyte solution containing the active material, and the redox flow battery can provide a redox flow battery with high energy density and good cycle characteristics. In addition, since the electrolyte solution of the present invention is an aqueous electrolyte solution, it is safer and easier to handle than organic solvent-based electrolyte solutions, and can be used in a wide range of applications.
Claims
1. A heterocyclic compound represented by the following formula (1), (2) or (3), or a salt thereof: [Formula 1] (In formula (1), R 1 ~R 8 are each independently a hydrogen atom, an acidic group, an alkoxy group, an alkyl group, an amino group, an amide group, or a group represented by formula (a), and R 1 ~R 8 At least one of the groups is a group represented by formula (a), X 1 is an oxygen atom, a sulfur atom or NY 2 represents Y 1 is a group represented by formula (b), Y 2 is a hydrogen atom, an alkyl group, a carbonyl group, a sulfonyl group, or a group represented by formula (b), R 9 and R 10 each independently represents a hydrogen atom or a substituent; Z 1 is an acidic group, n is an integer from 1 to 7; * a represents a bonding site to formula (1); * b is X in formula (a) 1 (representing the binding site with); [Case 2] (In formula (2), X 2 is an oxygen atom, a sulfur atom, or NR 11 and Y 2 is the linker, Z 2 is an acidic group, n 1 is an integer from 1 to 6, R 11 is a hydrogen atom or an alkyl group, R 12 are each independently an alkyl group or an acidic group, n 2 is an integer from 0 to 5; [C3] (In formula (3), X 3 is an oxygen atom or a sulfur atom, Y 3 is the linker, Z 3 is an acidic group, n 3 is an integer from 3 to 8, R 13 are each independently an alkyl group or an acidic group, n 4 is an integer from 0 to 5)
2. Z in the formula (b) 1 The heterocyclic compound or a salt thereof according to claim 1 , wherein is a sulfo group.
3. R in the formula (1) 1 ~R 8 The heterocyclic compound or a salt thereof according to claim 1 or 2, wherein at least two of the above are groups represented by formula (a).
4. R in the formula (1) 2 and R 3 The heterocyclic compound or a salt thereof according to any one of claims 1 to 3, wherein
5. An active material comprising at least one heterocyclic compound or a salt thereof according to any one of claims 1 to 4.
6. An electrolyte solution comprising the active material according to claim 5 .
7. The electrolyte according to claim 6, which is an electrolyte for a redox flow battery.
8. The electrolyte according to claim 6 or 7, wherein the content of water contained in the electrolyte is 1% by mass or more and 99.9% by mass or less.
9. The electrolyte according to claim 8, wherein the content of water contained in the electrolyte is 10% by mass or more and 99% by mass or less.
10. A redox flow battery comprising the electrolyte solution according to any one of claims 6 to 9.
11. 11. The redox flow battery of claim 10, further comprising an electrode and a membrane.