Insert material for liquid phase diffusion bonding and liquid phase diffusion bonding method

The insert material with eutectically reactive outer layers and a high-melting-point inner layer with low silicon content addresses the issue of silicon agglomeration in aluminum alloy bonding, enhancing joint strength by discharging silicon and preventing brittle failure.

JP7573242B2Active Publication Date: 2024-10-25TOYOTA JIDOSHA KK +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021116671
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-07-14
Publication Date
2024-10-25
Estimated Expiration
2041-07-14

AI Technical Summary

Technical Problem

Existing methods for liquid phase diffusion bonding of aluminum alloys containing silicon result in reduced bonding strength due to the agglomeration and coarsening of silicon phases at the joint, leading to brittle failure.

Method used

An insert material comprising a first and second outer layer made of metals or alloys that react eutectically with aluminum, an inner layer with lower silicon content and higher melting point, and optional surface layers that melt early to prevent silicon agglomeration, is used to sandwich the members to be bonded, allowing for eutectic reactions and discharge of silicon during bonding.

Benefits of technology

The insert material effectively suppresses silicon agglomeration, enhancing the bonding strength and preventing brittle failure by ensuring silicon is discharged from the joint, thereby improving the overall strength of the bonded aluminum alloy components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573242000001
    Figure 0007573242000001
  • Figure 0007573242000002
    Figure 0007573242000002
  • Figure 0007573242000003
    Figure 0007573242000003
Patent Text Reader

Abstract

To provide an insert material for liquid phase diffusion welding and a liquid phase diffusion welding method that can further improve welding strength of an aluminum alloy containing silicon.SOLUTION: An insert material 100 of the present disclosure comprises a first outside layer 21, an inside layer 10, and a second outside layer 22, in this order. The first outside layer 21 and the second outside layer 22 contain metal or the like that eutectically reacts with aluminum. The inside layer 10 contains metal or the like with a smaller mass content ratio of silicon than at least one aluminum alloy out of a first aluminum member 210 and a second aluminum member 220. The inside layer 10 has a higher melting point than the first outside layer 21 and the second outside layer 22. The inside layer 10 reacts eutectically with the first outside layer 21 and the second outside layer 22. In a liquid phase diffusion welding method of the present disclosure, the insert material 100 is used in applying liquid phase diffusion welding to the first aluminum member 210 and the second aluminum member 220.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an insert material for liquid phase diffusion bonding and a liquid phase diffusion bonding method, and more particularly to an insert material for liquid phase diffusion bonding of an aluminum alloy containing silicon and a liquid phase diffusion bonding method. [Background technology]

[0002] In recent years, from the viewpoint of protecting the global environment, there has been a demand for weight reduction in structural members used in transportation equipment and the like. For this reason, aluminum alloys have been increasingly used for structural members. In addition, various methods for joining aluminum alloys have been investigated.

[0003] For example, Non-Patent Document 1 discloses an insert material for liquid phase diffusion bonding based on a zinc sheet and a liquid phase diffusion bonding method for an aluminum alloy using the insert material. [Prior art documents] [Non-patent literature]

[0004] [Non-Patent Document 1] Hayato Shinohara and Shinji Koyama, "Effect of surface roughness on liquid phase diffusion bonding strength of Al alloy using Zn sheet with formate coating in air," Abstracts of the 13th JSME Conference on Production and Machine Tools, Vol. 13, C34, 2019. Summary of the Invention [Problem to be solved by the invention]

[0005] Non-Patent Document 1 discloses an insert material for liquid phase diffusion bonding made of a zinc sheet having a formate coating on its surface, and also discloses a method for liquid phase diffusion bonding of an aluminum alloy containing silicon using the insert material.

[0006] Non-Patent Document 1 discloses that by providing a formate coating on the surface of a zinc sheet, the oxide film is replaced with formate, the oxide film on the bonding surface is removed, and reoxidation of the bonding surface can be prevented. Non-Patent Document 1 also discloses that the bonding strength is improved when an aluminum alloy is liquid phase diffusion bonded using such an insert material.

[0007] However, when the aluminum alloy contains silicon, although the bonding strength is improved, the degree of the improvement is reduced. For this reason, the present inventors have found a problem that a further improvement in the bonding strength is desired when liquid phase diffusion bonding an aluminum alloy containing silicon.

[0008] The present disclosure has been made to solve the above problems. That is, an object of the present disclosure is to provide an insert material for liquid phase diffusion bonding and a liquid phase diffusion bonding method that can further improve the bonding strength of an aluminum alloy containing silicon. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to achieve the above object, and have completed the insert material for liquid phase diffusion bonding and the liquid phase diffusion bonding method of the present disclosure. The insert material for liquid phase diffusion bonding and the liquid phase diffusion bonding method of the present disclosure include the following aspects. <1> An insert material for liquid phase diffusion bonding of a first aluminum member and a second aluminum member, at least one of which is made of an aluminum alloy containing silicon, a first outer layer, an inner layer, and a second outer layer, in that order; the first outer layer and the second outer layer are made of a metal or alloy that reacts eutectic with aluminum; the inner layer is made of a metal or alloy having a lower mass content of silicon than the aluminum alloy of at least one of the first aluminum member and the second aluminum member; the inner layer has a higher melting point than the first outer layer and the second outer layer; and the inner layer reacts eutectic with the first outer layer and the second outer layer; Insert material for liquid phase diffusion bonding. <2> The insert material for liquid phase diffusion bonding described in <1>, wherein at least one of the first outer layer and the second outer layer is composed of metallic zinc or a zinc alloy. <3> The insert material for liquid phase diffusion bonding according to <1> or <2>, wherein the inner layer is made of metallic aluminum or an aluminum alloy. <4> A surface layer is further provided on the outside of at least one of the first outer layer and the second outer layer, The surface layer has a lower melting point than the first outer layer and the second outer layer, and is made of a metal or alloy that melts by itself or reacts eutectic with aluminum. The insert material for liquid phase diffusion bonding according to any one of <1> to <3>. <5> The insert material for liquid phase diffusion bonding according to <4>, wherein the surface layer is composed of one or more selected from the group consisting of metallic tin, metallic bismuth, metallic indium, metallic gallium, a tin alloy, a bismuth alloy, an indium alloy, and a gallium alloy. <6> The insert material for liquid phase diffusion bonding according to any one of <1> to <5>, wherein at least one of the first outer layer and the second outer layer is provided on one or both sides with one or more coatings selected from the group consisting of a formate coating, an acetate coating, a citrate coating, and a tartrate coating. <7> A method for liquid phase diffusion bonding of a first aluminum member and a second aluminum member, at least one of which is made of an aluminum alloy containing silicon, comprising: laminating a first outer layer, an inner layer, and a second outer layer in this order to obtain an insert material; disposing the insert material between the first aluminum member and the second aluminum member; and applying a load to the insert material through at least one of the first aluminum member and the second aluminum member while heating the first aluminum member, the second aluminum member, and the insert material, thereby liquid phase diffusion bonding the first aluminum member and the second aluminum member; Including, the first outer layer and the second outer layer are made of a metal or alloy that reacts eutectic with aluminum, the inner layer is made of a metal or alloy having a lower mass content of silicon than the aluminum alloy of at least one of the first aluminum member and the second aluminum member; the inner layer has a higher melting point than the first outer layer and the second outer layer; and the inner layer reacts eutectic with the first outer layer and the second outer layer; Liquid phase diffusion bonding method. <8> The liquid phase diffusion bonding method according to <7>, wherein at least one of the first outer layer and the second outer layer is made of metallic zinc or a zinc alloy. <9> The liquid phase diffusion bonding method according to <7> or <8>, wherein the inner layer is made of metallic aluminum or an aluminum alloy. <10> A surface layer is further laminated on the outside of at least one of the first outer layer and the second outer layer to obtain an insert material. Including, The surface layer has a lower melting point than the first outer layer and the second outer layer, and is made of a metal or alloy that melts by itself or reacts eutectic with aluminum. The liquid phase diffusion bonding method according to any one of items <7> to <9>. <11> The liquid phase diffusion bonding method according to <10>, wherein the surface layer is made of at least one material selected from the group consisting of metallic tin, metallic bismuth, metallic indium, metallic gallium, a tin alloy, a bismuth alloy, an indium alloy, and a gallium alloy. <12> The liquid phase diffusion bonding method according to any one of <7> to <11>, further comprising forming one or more coatings selected from the group consisting of a formate coating, an acetate coating, a citrate coating, and a tartrate coating on one or both surfaces of at least one of the first outer layer and the second outer layer to obtain an insert material. Effect of the Invention

[0010] According to the present disclosure, an insert material in which a metal or alloy having a lower silicon content than the aluminum alloy of the members to be joined is sandwiched between a metal or alloy that undergoes a eutectic reaction with aluminum can prevent coarse agglomerates of silicon originating from the members to be joined from remaining at the joint. As a result, according to the present disclosure, it is possible to provide an insert material for liquid phase diffusion bonding and a liquid phase diffusion bonding method that can further improve the bonding strength of an aluminum alloy containing silicon by preventing coarse agglomerates from remaining at the joint. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a cross-sectional schematic diagram showing one embodiment of an insert material for liquid phase diffusion bonding according to the present disclosure. [Diagram 2] FIG. 2 is a cross-sectional schematic diagram showing one embodiment of the liquid phase diffusion bonding method of the present disclosure. [Diagram 3] FIG. 3 is a cross-sectional schematic view showing another embodiment of the insert material for liquid phase diffusion bonding according to the present disclosure. [Figure 4] FIG. 4 is a schematic cross-sectional view showing one embodiment of an insert material for liquid phase diffusion bonding according to the present disclosure, which has formate coatings on the surfaces of the first outer layer and the second outer layer. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing another embodiment of an insert material for liquid phase diffusion bonding according to the present disclosure, which has formate coatings on the surfaces of the first outer layer and the second outer layer. [Figure 6] FIG. 6 is a graph showing the change over time in bonding pressure and bonding temperature during liquid phase diffusion bonding. [Figure 7] FIG. 7 is an SEM image of the bonded portion of the sample of Example 1. [Figure 8]FIG. 8 is an SEM image of the joint of the sample of Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the insert material for liquid phase diffusion bonding and the liquid phase diffusion bonding method according to the present disclosure will be described in detail. Note that the insert material for liquid phase diffusion bonding and the liquid phase diffusion bonding method according to the present disclosure are not limited to the following embodiments.

[0013] Without being bound by theory, the reason why the bonding strength is further improved when the insert material for liquid phase diffusion bonding of the present disclosure is used to bond an aluminum alloy to silicon-containing aluminum alloy will be described with reference to the drawings. In the following description, the insert material for liquid phase diffusion bonding of the present disclosure may be simply referred to as the "insert material of the present disclosure."

[0014] Fig. 1 is a cross-sectional schematic diagram showing one embodiment of an insert material according to the present disclosure, and Fig. 2 is a cross-sectional schematic diagram showing one embodiment of a liquid phase diffusion bonding method according to the present disclosure.

[0015] As shown in Fig. 1, the insert material 100 of the present disclosure (hereinafter sometimes simply referred to as "insert material 100") comprises a first outer layer 21, an inner layer 10, and a second outer layer 22, in this order. Then, as shown in Fig. 2, the insert material 100 of the present disclosure is sandwiched between a first aluminum member 210 and a second aluminum member 220, and the first aluminum member 210 and the second aluminum member 220 are liquid phase diffusion bonded. In other words, the first aluminum member 210 and the second aluminum member 220 are members to be joined.

[0016] When the insert material is used to perform liquid phase diffusion bonding of the members to be joined, at least a part of the insert material melts and becomes liquid. Then, at least a part of the liquid phase and at least a part of the members to be joined diffuse into each other at the site where the liquid phase contacts the members to be joined and in the vicinity thereof, thereby bonding the members to be joined.

[0017] In the case of the embodiment shown in FIG. 2, when the first aluminum member 210 and the second aluminum member 220 are liquid phase diffusion bonded using the insert material 100, at least a part of the insert material 100 melts to form a liquid phase. Then, the liquid phase and the first aluminum member 210 interdiffuse at the portion where the liquid phase contacts the first aluminum member 210 and in the vicinity thereof. Similarly, the liquid phase and the second aluminum member 220 interdiffuse at the portion where the liquid phase contacts the second aluminum member 220 and in the vicinity thereof. At this time, at least a part of the first outer layer 21 and at least a part of the second outer layer 22 of the insert material 100 are melted to form a liquid phase. Therefore, the first outer layer 21 and the second outer layer 22 are composed of a metal or alloy that reacts eutectic with aluminum. As a result, during bonding, mainly at least a part of the insert material 100, more specifically, at least a part of the first outer layer 21 and at least a part of the second outer layer 22 melt to form a liquid phase. The phrase "mainly at least a portion of the insert material 100 melts to form a liquid phase" means that other than at least a portion of the insert material 100 may also melt to form a liquid phase. Specifically, it means that at least a portion of the insert material 100 melts to form a liquid phase, and the liquid phase may form a part of the portion interdiffusing with the first aluminum member 210 and the second aluminum member 220. This is because the melting point of the interdiffusing portion is lowered due to the interdiffusion.

[0018] In the case where the first aluminum member 210 contains silicon, when at least a part of the insert material 100 forms a liquid phase, silicon in the first aluminum member 210 is dissolved and discharged into the liquid phase. Similarly, in the case where the second aluminum member 220 contains silicon, when at least a part of the insert material 100 forms a liquid phase, silicon in the second aluminum member 220 is dissolved and discharged into the liquid phase. At this time, if the insert material 100 does not have the inner layer 10, the liquid phase portion solidifies while silicon remains in the insert material 100. During the solidification, a phase containing a large amount of silicon (hereinafter, simply referred to as "silicon phase") remains in an aggregated and coarse state. The present inventors have found that if the aggregated and coarse silicon phase remains in the joint between the first aluminum member 210 and the second aluminum member 220, the joint strength decreases. Although not bound by theory, it is considered that the aggregated and coarse silicon phase causes brittle fracture of the joint because the silicon phase is a hard phase.

[0019] The present inventors have found that in order to prevent the aggregated and coarsened silicon phase from remaining in the joint, it is sufficient to dispose the inner layer 10 between the first outer layer 21 and the second outer layer 22 of the insert material 100. The present inventors have also found that it is sufficient for the inner layer 10 to contain a metal or alloy having a lower mass content of silicon than the aluminum alloy of at least one of the first aluminum member 210 and the second aluminum member 220. Furthermore, the present inventors have found that it is sufficient for the inner layer 10 to have a higher melting point than the first outer layer 21 and the second outer layer 22, and for the inner layer 10 to undergo a eutectic reaction with the first outer layer 21 and the second outer layer 22.

[0020] When the first aluminum member 210 and the second aluminum member 220 are subjected to liquid phase diffusion bonding, a load that compresses the insert material 100 is applied by the first aluminum member 210 and the second aluminum member 220 .

[0021] When silicon eluted from the first aluminum member 210 and the second aluminum member 220 starts to be discharged into the liquid phase in which at least a portion of the first outer layer 21 and the second outer layer 22 are melted, it is considered that the inner layer 10 maintains a solid phase. This is because the inner layer 10 has a higher melting point than the first outer layer 21 and the second outer layer 22. When a load that compresses the insert material 100 is applied in this state, it is considered that the liquid phase is discharged to the outside of the insert material 100 along the inner layer 10 (along the left-right direction in FIG. 2).

[0022] When the liquid phase originating from the first outer layer 21 and the second outer layer 22 is discharged along the inner layer 10, the inner layer 10 gradually melts from its outer side (the side in contact with the first outer layer 21 and the second outer layer 22) by eutectic reaction as the liquid phase diffusion bonding progresses, and forms a liquid phase. It is considered that the liquid phase originating from the inner layer 10 is also discharged to the outside of the insert material 100. The inner layer 10 has a smaller mass content of silicon than at least one of the aluminum alloys of the first aluminum member 210 and the second aluminum member 220. Therefore, even if a part of the liquid phase originating from the inner layer 10 starts to solidify and forms a silicon phase while being discharged to the outside of the insert material 100, the amount of the silicon phase formed is small. For this reason, the silicon phase hardly hinders the liquid phase originating from the inner layer 10 from being discharged to the outside of the insert material 100, and rather, it is considered that the silicon phase is also discharged to the outside of the insert material 100 together with the unsolidified liquid phase. In this way, it is believed that it is possible to avoid or suppress the presence of aggregated and coarsened silicon at the bonded portion between the first aluminum member 210 and the second aluminum member 220 after liquid phase diffusion bonding, and the bonding strength between the first aluminum member and the second aluminum member 220 can be further improved.

[0023] Next, the constituent elements of the insert material and the liquid phase diffusion bonding method of the present disclosure, which have been completed based on the findings and the like described above, will be described.

[0024] <Insert material for liquid phase diffusion bonding> 2, the insert material 100 of the present disclosure is used by being sandwiched between a first aluminum member 210 and a second aluminum member 220. The first aluminum member 210 and the second aluminum member 220 will be described in detail in “<Liquid phase diffusion bonding method>”.

[0025] As shown in Fig. 1, the insert material 100 of the present disclosure includes a first outer layer 21, an inner layer 10, and a second outer layer 22 in this order. Fig. 3 is a schematic cross-sectional view showing another embodiment of the insert material of the present disclosure. As shown in Fig. 3, the insert material 100 of the present disclosure may further include a first surface layer 31 and a second surface layer 32 on the outside of the first outer layer 21 and the second outer layer 22. Each of these layers included in the insert material 100 of the present disclosure will be described in detail below.

[0026] <Inner layer> The inner layer 10 is disposed between the first outer layer 21 and the second outer layer 22. The inner layer 10 is composed of a metal or alloy having a lower mass content of silicon than the aluminum alloy of the members to be joined. As described above, this makes it possible to avoid or suppress the aggregation and coarsening of silicon originating from the inner layer at the joint after liquid phase diffusion bonding. Here, "composed of a metal or alloy having a low mass content of silicon" means that a composition other than the desired metal or alloy may be contained, and the content of the desired metal or alloy may be, for example, 95% or more, 96% or more, 97% or more, 98% or more, or 99% or more by mass.

[0027] At least one of the members to be joined, i.e., the first aluminum member 210 and the second aluminum member 220, is made of an aluminum alloy containing silicon. Therefore, the inner layer 10 is made of a metal or alloy having a lower mass content of silicon than the aluminum alloy of at least one of the first aluminum member 210 and the second aluminum member 220. In this specification and the like, unless otherwise specified, "metal" means an unalloyed metal, and "alloy" means a composition containing two or more elements that are alloyed with each other.

[0028] The inner layer 10 has a higher melting point than the first outer layer 21 and the second outer layer 22. As a result, as described above, when silicon eluted from the first aluminum member 210 and the second aluminum member 220 starts to be discharged into the liquid phase in which at least a part of the first outer layer 21 and the second outer layer 22 are melted, the inner layer 10 can maintain a solid phase. Then, the liquid phase derived from the first outer layer 21 and the second outer layer 22 is discharged outside the insert material 100 along the inner layer 10. In this way, it is possible to prevent or suppress the silicon discharged from the first aluminum member 210 and the second aluminum member 220 to the first outer layer 21 and the second outer layer 22 from agglomerating and coarsening and remaining in the joint portion after liquid phase diffusion bonding.

[0029] The inner layer 10 undergoes a eutectic reaction with the first outer layer 21 and the second outer layer 22. As a result, as described above, the inner layer 10, which maintained a solid phase at the beginning of the liquid phase diffusion bonding, gradually undergoes a eutectic reaction from the outside with the liquid phase derived from the first outer layer 21 and the second outer layer 22, and the inner layer 10 itself also gradually becomes liquid from the outside. Then, most of the liquid phase derived from the inner layer 10 is discharged to the outside of the insert material 100.

[0030] The inner layer 10 as described above is typically made of metallic aluminum, that is, aluminum that is not alloyed with metals other than aluminum. The purity of metallic aluminum may be 90% or more, 95% or more, 97% or more, 98% or more, or 99% or more, by mass %, or may be 100%. For example, metallic aluminum with a purity of 90% or more contains 90% or more of aluminum, with the remainder being unavoidable impurities. The same applies to the case where the purity is 95% or more, 97% or more, 98% or more, or 99% or more. In this specification, the term "unavoidable impurities" refers to impurities contained in raw materials or impurities mixed in during the manufacturing process, which cannot be avoided, or which would result in a significant increase in manufacturing costs if avoided. Impurities mixed in during the manufacturing process include substances that are included within a range that does not affect the bonding strength, etc., due to manufacturing reasons.

[0031] The inner layer 10 is made of an aluminum alloy having a lower mass content of silicon than the aluminum alloy of at least one of the first aluminum member 210 and the second aluminum member 220. As described above, this makes it possible to avoid or suppress the presence of aggregated and coarsened silicon phases originating from the inner layer 10 remaining in the bonded portion after liquid phase diffusion bonding. The composition of the aluminum alloy constituting at least one of the first aluminum member 210 and the second aluminum member 220 will be described later. The difference between the silicon content of the aluminum alloy constituting at least one of the first aluminum member 210 and the second aluminum member 220 and the silicon content of the aluminum alloy contained in the inner layer 10 may be, for example, 0.1% or more, 0.5% or more, 1% or more, or 2% or more in mass%, and may be 30%, 25% or less, 20% or less, 15% or less, 10% or less, or 5% or less.

[0032] The thickness of the inner layer 10 may be appropriately determined in consideration of the liquid phase diffusion bonding conditions, etc., so that the inner layer 10 remains in the bonded portion after liquid phase diffusion bonding to an extent that does not adversely affect the bond strength, or so that the inner layer 10 does not remain in the bonded portion after liquid phase diffusion bonding. The thickness of the inner layer 10 may be 0.2 mm or more, 0.3 mm or more, 0.4 mm or more, or 0.5 mm or more, and may be 1.2 mm or less, 1.0 mm or less, 0.8 mm or less, or 0.6 mm or less.

[0033] First outer layer and second outer layer The first outer layer 21 and the second outer layer 22 are disposed on the outside of the inner layer 10 with the inner layer 10 sandwiched therebetween.

[0034] The first outer layer 21 and the second outer layer 22 undergo a eutectic reaction with aluminum in the first aluminum member 210 and the second aluminum member 220, causing the first outer layer 21 and the second outer layer 22 to melt and form a liquid phase. This liquid phase then diffuses into the first aluminum member 210 and the second aluminum member 220, and the first aluminum member 210 and the second aluminum member are liquid phase diffusion bonded together. For this reason, the first outer layer 21 and the second outer layer 22 are composed of a metal or alloy that undergoes a eutectic reaction with aluminum. Here, "composed" means that the composition may contain a composition other than the desired metal or alloy, and the content of the desired metal or alloy may be, for example, 95% or more, 96% or more, 97% or more, 98% or more, or 99% or more by mass%.

[0035] The first outer layer 21 and the second outer layer 22 as described above are typically made of metallic zinc. The purity of metallic zinc may be, in mass %, 90% or more, 95% or more, 97% or more, 98% or more, or 99% or more, or may be 100%. For example, metallic zinc with a purity of 90% or more can be said to contain 90% or more of zinc, with the remainder being unavoidable impurities. The same applies when the purity is 95% or more, 97% or more, 98% or more, or 99% or more.

[0036] The first outer layer 21 and the second outer layer 22 may be made of a zinc alloy. The zinc alloy refers to a composition containing, in addition to zinc, an element that alloys with zinc. The content of such an alloying element may be, in mass%, 0.1% or more, 0.5% or more, 1% or more, or 3% or more, and may be 15% or less, 10% or less, 7% or less, or 5% or less. When a plurality of alloying elements are contained, the content is the total content of the alloying elements. Examples of such alloying elements include copper, aluminum, titanium, lead, tin, cadmium, and iron. It can be said that such a zinc alloy contains, in mass%, 0.1 to 15% of an alloying element, with the remainder being zinc and unavoidable impurities.

[0037] The thicknesses of the first outer layer 21 and the second outer layer 22 may be appropriately determined in consideration of the liquid phase diffusion bonding conditions, etc., so that substances derived from the first outer layer 21 and the second outer layer 22 do not remain in the bonded portion after liquid phase diffusion bonding and do not adversely affect the bonding strength. The thicknesses of the first outer layer 21 and the second outer layer 22 may be 0.2 mm or more, 0.4 mm or more, or 0.6 mm, and may be 1.6 mm or less, 1.4 mm or less, 1.2 mm or less, 1.0 mm or less, or 0.8 mm or less.

[0038] The first outer layer 21 and the second outer layer 22 may be made of the same material or different materials, so long as each layer satisfies the above-mentioned requirements.

[0039] <First surface layer and second surface layer> As shown in Fig. 3, the insert material 100 of the present disclosure may optionally include a surface layer 30 on the outside of the first outer layer 21 and the second outer layer 22. Typically, as shown in Fig. 3, the insert material 100 shown in Fig. 1 includes a first surface layer 31 and a second surface layer 32 on both outsides, but may include only one of them. That is, the insert material 100 of the present disclosure may further include a surface layer 30 on the outside of at least one of the first outer layer 21 and the second outer layer 22.

[0040] The first surface layer 31 and the second surface layer 32 are made of a metal or alloy that has a lower melting point than the first outer layer 21 and the second outer layer 22 and reacts eutectic with aluminum. As a result, during liquid phase diffusion bonding, the first surface layer 31 and the second surface layer 32 melt only by themselves, or react eutectic with aluminum in the first aluminum member 210 and the second aluminum member 220, and melt earlier than the first outer layer 21 and the second outer layer 22 to form a liquid phase. The liquid phase surrounds the bonding surfaces of the first aluminum member 210 and the second aluminum member, and it is possible to prevent or suppress the bonding surfaces from coming into contact with the external atmosphere. As a result, it is possible to prevent or suppress the bonding portions from being oxidized during liquid phase diffusion bonding. In addition, when the first surface layer 31 and the second surface layer 32 are made of metal tin or a tin alloy, since metal tin and tin alloy are soft, metal tin or tin alloy penetrates into the minute irregularities on the surfaces of the first aluminum member 210 and the second aluminum member 220. In this case, air present in the minute asperities is expelled and the air is prevented from entering the minute asperities again during bonding, thereby contributing to the suppression of oxidation of the bonded portion. Note that "comprises" means that a composition other than the desired metal or alloy may be contained, and the content of the desired metal or alloy may be, for example, 95% or more, 96% or more, 97% or more, 98% or more, or 99% or more by mass.

[0041] In an embodiment in which the insert material 100 of the present disclosure includes the first surface layer 31 and the second surface layer 32, the first surface layer 31 and the second surface layer 32 melt and form a liquid phase at the beginning of the liquid phase diffusion bonding (hereinafter, this liquid phase may be referred to as the "liquid phase originating from the first surface layer 31 and the second surface layer 32"). Then, as the liquid phase diffusion bonding progresses, the first outer layer 21 and the second outer layer 22 melt and form a liquid phase (hereinafter, this liquid phase may be referred to as the "liquid phase originating from the first outer layer 21 and the second outer layer 22"). In this embodiment, as the liquid phase diffusion bonding progresses, the liquid phase originating from the first surface layer 31 and the second surface layer 32 is discharged to the outside of the insert material 100 along the first outer layer 21 and the second outer layer 22 before the liquid phase originating from the first outer layer 21 and the second outer layer 22 is formed.

[0042] The first surface layer 31 and the second surface layer 32 are composed of, for example, metallic tin, metallic bismuth, metallic indium, or metallic gallium, and are typically composed of metallic tin. The purity of metallic tin may be, in mass %, 90% or more, 95% or more, 97% or more, 98% or more, or 99% or more, or may be 100%. For example, metallic tin with a purity of 90% or more contains 90% or more of tin, with the remainder being unavoidable impurities. The same is true when the purity is 95% or more, 97% or more, 98% or more, or 99% or more. The same is true for metallic bismuth, metallic indium, and metallic gallium.

[0043] The first surface layer 31 and the second surface layer 32 may be made of a tin alloy. The tin alloy means a composition containing, in addition to tin, an element that alloys with tin. The content of such an alloying element may be, in mass%, 0.1% or more, 0.5% or more, 1% or more, or 3% or more, and may be 15% or less, 10% or less, 7% or less, or 5% or less. When a plurality of alloying elements are contained, the content is the total content of the alloying elements. Examples of such alloying elements include copper, aluminum, titanium, lead, zinc, cadmium, and iron. It can be said that such a tin alloy contains, in mass%, 0.1 to 15% of an alloying element, with the remainder being tin and unavoidable impurities.

[0044] The thickness of the first surface layer 31 and the second surface layer 32 may be appropriately determined in consideration of the liquid phase diffusion bonding conditions, etc., so that substances derived from the first surface layer 31 and the second surface layer 32 do not remain in the bonded portion after liquid phase diffusion bonding and adversely affect the bonding strength. The thickness of the first surface layer 31 and the second surface layer 32 may be 0.005 mm or more, 0.006 mm or more, or 0.007 mm or more, and may be 1.6 mm or less, 1.4 mm or less, 1.2 mm or less, 1.0 mm or less, 0.80 mm or less, 0.60 mm or less, 0.40 mm or less, 0.20 mm or less, 0.10 mm or less, 0.080 mm or less, 0.040 mm or less, 0.020 mm or less, 0.010 mm or less, 0.009 mm or less, or 0.008 mm or less.

[0045] As long as the first surface layer 31 and the second surface layer 32 each satisfy the above-mentioned requirements, the first surface layer 31 and the second surface layer 32 may be made of the same material or different materials.

[0046] <Formate coating, etc.> At least one of the first outer layer 21 and the second outer layer 22 may have a formate coating 40 on one or both sides. Fig. 4 is a cross-sectional schematic diagram showing one embodiment in which the first outer layer and the second outer layer have a formate coating on both sides. Fig. 5 is a cross-sectional schematic diagram showing another embodiment in which the first outer layer and the second outer layer have a formate coating 40 on both sides.

[0047] In the embodiment shown in FIG. 4, the first formate coating 41 and the second formate coating 42 are provided on both sides of the first outer layer 21 and the second outer layer 22, respectively, but the present invention is not limited thereto. For example, the first formate coating 41 may be provided only on both sides of the first outer layer 21, and the second formate coating 42 may not be provided on the surface of the second outer layer 22. In the embodiment shown in FIG. 4, the first formate coating 41 is provided on both sides of the first outer layer 21, but the first formate coating 41 may be provided only on one side. Alternatively, for example, as in the embodiment shown in FIG. 5, the first surface layer 31 and the second surface layer 32 may be provided on the outside of the first formate coating 41 and the second formate coating 42. In the embodiment shown in FIG. 5, both the first surface layer 31 and the second surface layer 32 are provided, but the present invention is not limited thereto, and only one of the first surface layer 31 and the second surface layer 32 may be provided.

[0048] When at least one of the first outer layer 21 and the second outer layer 22 has the formate coating 40 on at least one surface thereof, the oxide film on the bonding surface can be removed, and reoxidation of the bonding surface can be avoided or suppressed. This can improve the bonding strength. Without being bound by theory, it is believed that this is because the formate coating is thermally decomposed during liquid phase diffusion bonding, which makes it easier to cause a eutectic reaction with the bonding surfaces of the first aluminum member 210 and the second aluminum member 220.

[0049] Examples of coatings that function similarly to the formate coating include acetate coatings, citrate coatings, and tartrate coatings. Therefore, at least one of the first outer layer and the second outer layer may have one or more coatings selected from the group consisting of formate coatings, acetate coatings, citrate coatings, and tartrate coatings on one or both sides. Details of formate coatings and the like will be described in "Liquid Phase Diffusion Bonding Method". For details of formate coatings, see Non-Patent Document 1.

[0050] <<Liquid Phase Diffusion Bonding Method>> Next, the liquid phase diffusion bonding method of the present disclosure will be described. As shown in FIG. 2, the liquid phase diffusion bonding method of the present disclosure bonds a first aluminum member 210 and a second aluminum member 220. In this specification, unless otherwise specified, the "aluminum member" means at least one of a metal aluminum member and an aluminum alloy member. Note that the following description of the first aluminum member 210 and the second aluminum member 220 can also be applied to the above-mentioned insert material 100 of the present disclosure. Hereinafter, the members to be bonded, that is, the first aluminum member and the second aluminum member, will be described.

[0051] <First aluminum member and second aluminum member> In the liquid phase diffusion bonding method of the present disclosure, at least one of the first aluminum member 210 and the second aluminum member is made of an aluminum alloy containing silicon. "Made of an aluminum alloy containing silicon" means that it may contain a composition other than an aluminum alloy containing silicon. For example, when both the first aluminum member 210 and the second aluminum member 220 are made of an aluminum alloy containing silicon, the content ratio of the aluminum alloy containing silicon in each of the first aluminum member 210 and the second aluminum member 220 may be, for example, 95% or more, 96% or more, 97% or more, 98% or more, or 99% or more by mass.

[0052] According to the liquid phase diffusion method of the present disclosure, it is possible to prevent or suppress coarse silicon agglomerates originating from the silicon-containing aluminum alloy in the first aluminum member 210 or the second aluminum member 220 from remaining in the joint.

[0053] If the aluminum alloy in the first aluminum member 210 or the second aluminum member 220 contains even a small amount of silicon, there is a possibility that silicon coarse aggregates remain in the joint, and the effect of the liquid phase diffusion bonding method of the present disclosure can be enjoyed. Typically, aluminum alloys containing silicon are aluminum alloys for wrought materials and castings that contain silicon. The aluminum alloys for wrought materials include aluminum alloys for forging, and the aluminum alloys for castings include aluminum alloys for die casting. Therefore, in the aluminum alloys containing silicon, the content of silicon may be, for example, 0.1% or more, 0.5% or more, 0.7% or more, 1.0% or more, 1.5% or more, 2.0% or more, 4.0% or more, 6.0% or more, or 8.0% or more, in mass%, and may be 24.0% or less, 22.0% or less, 20.0% or less, 18.0% or less, 16.0% or less, 14.0% or less, 12.0% or less, or 10.0% or less. Both the wrought aluminum alloy and the cast aluminum alloy may contain, in addition to silicon, for example, copper, magnesium, zinc, iron, manganese, nickel, titanium, lead, tin, chromium, etc., depending on the application, in order to improve age hardenability, corrosion resistance, heat resistance, and / or wear resistance, etc. The total content of those elements other than silicon may be, for example, 0.05% or more, 0.1% or more, 0.5% or more, 1.0% or more, 3.0% or more, or 5.0% or more, and 15.0% or less, 13.0% or less, 10.0% or less, or 7.0% or less, in mass%, and the balance may be aluminum and unavoidable impurities.

[0054] The liquid phase diffusion bonding of the present disclosure is particularly useful when at least one of the first aluminum member 210 and the second aluminum member has a high silicon content, such as an aluminum alloy for casting. Thus, in an aluminum alloy containing silicon, the silicon content, by mass%, may be 4.0% or more, 6.0% or more, or 8.0% or more, and 24.0% or less, 22.0% or less, 20.0% or less, 18.0% or less, 16.0% or less, 14.0% or less, 12.0% or less, or 10.0% or less.

[0055] Examples of the aluminum alloy for wrought materials include alloys containing, by mass%, 0.01-5.0% copper, 0.1-1.5% silicon, 0.01-3.0% magnesium, 0-2.0% zinc, iron, manganese, nickel, titanium, lead, tin, and chromium in total, with the remainder being aluminum and unavoidable impurities. In particular, the aluminum alloy for wrought materials may be, for example, the 1000 series, 2000 series, 3000 series, 4000 series, 6000 series, or 7000 series of the Japanese Industrial Standards, and in particular the 4000 series, 6000 series, or 7000 series.

[0056] Examples of the aluminum alloy for casting include alloys containing, by mass%, 0.10-5.0% copper, 4.0-24.0% silicon, 0.1-2.0% magnesium, 0-5.0% zinc, iron, manganese, nickel, titanium, lead, tin, and chromium in total, with the balance being aluminum and unavoidable impurities. In particular, the aluminum alloy for casting may be, for example, AC2A, AC2B, AC2C, AC3A, AC4B, AC4C, AC4CH, AC4D, AC8A, AC8B, AC8C, AC9A, or AC9B, etc., according to the Japanese Industrial Standards.

[0057] In particular, AC2C may contain, for example, by mass%, 0.5-1.1% copper, 6.5-7.5% silicon, 0.2-0.4% magnesium, 0-0.1% zinc, 0-0.1% manganese, 0-0.1% nickel, and 0-0.1% tin, with the remainder being aluminum and unavoidable impurities. In this specification, unless otherwise specified, 0% means that the component may not be contained.

[0058] The aluminum alloy for casting may be an alloy for die casting, for example, an alloy containing, by mass%, 0.10-5.0% copper, 5.0-20.0% silicon, 0-2.0% magnesium, 0-5.0% zinc, iron, manganese, nickel, titanium, lead, tin, and chromium in total, with the balance being aluminum and unavoidable impurities. In particular, the aluminum alloy for die casting may be, for example, ADC3, ADC10, ADC10Z, ADC12, ADC12Z, or ADC14, etc., of the Japanese Industrial Standards, and particularly, ADC10, ADC12, and ADC14, etc.

[0059] In particular, ADC12 may contain, for example, by mass%, 1.5 to 3.5% copper, 9.6 to 12.0% silicon, 0 to 0.3% magnesium, 0 to 0.3% zinc, 0 to 0.5% magnesium, 0 to 0.5% nickel, and 0 to 0.3% tin, with the remainder being aluminum and unavoidable impurities.

[0060] In the liquid phase diffusion bonding method of the present disclosure, the first aluminum member 210 and the second aluminum member 220 described above are bonded as follows.

[0061] The liquid phase diffusion bonding method of the present disclosure includes an insert material preparation step and a liquid phase diffusion bonding step. The liquid phase diffusion bonding method of the present disclosure may also include a surface layer addition step and a formate coating or the like addition step, as desired. Each of these steps will be described below.

[0062] <Insert material preparation process> As shown in FIG. 1, the insert material 100 is obtained by laminating a first outer layer 21, an inner layer 10, and a second outer layer 22 in this order.

[0063] There are no particular limitations on the lamination method as long as the first outer layer 21, the inner layer 10, and the second outer layer 22 can be laminated without any gaps.

[0064] Examples of the lamination method include preparing plate materials and / or foil materials for each layer of the first outer layer 21, the inner layer 10, and the second outer layer 22, and laminating them. It is preferable to clean the surfaces of the plate materials and / or foil materials for each layer by degreasing and / or polishing, etc., before lamination. This makes it possible to avoid or suppress oxides and / or inclusions remaining in the joint, and as a result, it is possible to improve the joint strength.

[0065] Alternatively, the lamination method may include forming a first outer layer 21 and a second outer layer 22 on both outer surfaces of the inner layer 10. The deposition method is not particularly limited as long as the layers, particularly the inner layer 10, are not altered during deposition. The deposition method may include a thermal spray method, a plating method, a deposition method, etc. When the deposition method is used, it is relatively easy to laminate the layers without gaps, which leads to improved bonding strength. In addition, the layers do not separate, which is advantageous for handling the insert material.

[0066] Lamination of the plate material and / or foil material and film formation may be combined. For example, the first outer layer 21 may be formed on one surface of the inner layer 10, and the plate material and / or foil material of the second outer layer 22 may be laminated on the other surface of the inner layer 10.

[0067] The material (composition), thickness, etc. of each of the first outer layer 21, the inner layer 10, and the second outer layer 22 are as described in "<Insert Material for Liquid Phase Diffusion Bonding>".

[0068] <Liquid Phase Diffusion Bonding Process> 2, the insert material 100 is placed between the first aluminum member 210 and the second aluminum member 220. Then, while the first aluminum member 210, the second aluminum member 220, and the insert material 100 are heated, a load is applied to the insert material 100 via at least one of the first aluminum member 210 and the second aluminum member 220. In this manner, the first aluminum member 210 and the second aluminum member 220 can be liquid phase diffusion bonded.

[0069] The liquid phase diffusion bonding temperature may be appropriately determined so that the first outer layer 21 and the second outer layer 22 undergo a eutectic reaction with the aluminum in the first aluminum member 210 and the second aluminum member 220 and is equal to or lower than the melting point of the inner layer 10. When the first outer layer 21 and the second outer layer 22 are made of metallic zinc and the inner layer 10 is made of metallic aluminum, the liquid phase diffusion bonding temperature may be, for example, 380° C. or more, 400° C. or more, or 450° C. or more, and may be 660° C. or less, 650° C. or less, 600° C. or less, 550° C. or less, or 500° C. or less.

[0070] The liquid phase diffusion bonding pressure may be appropriately determined so as to be equal to or higher than the pressure at which the insert material 100 is not displaced when sandwiched between the first aluminum member 210 and the second aluminum member, and equal to or lower than the pressure at which the bonded portion is not significantly deformed. The liquid phase diffusion bonding pressure may typically be 1 MPa or more, 2 MPa or more, 3 MPa or more, or 4 MPa or more, and may be 25 MPa or less, 20 MPa or less, 15 MPa or less, 10 MPa or less, or 5 MPa or less.

[0071] The liquid phase diffusion bonding time may be appropriately determined based on the time at which the insert material 100, particularly the first outer layer 21 and the second outer layer 22, are concentrated and do not remain in the bonded portion. When the liquid phase diffusion bonding temperature is equal to or higher than the solution (solid solution) temperature of the first aluminum member 210 and the second aluminum member 220, the liquid phase diffusion bonding time can be determined in consideration of the solution (solid solution) of the first aluminum member 210 and the second aluminum member 220. The liquid phase diffusion bonding time may be, for example, 10 minutes or more, 30 minutes or more, 60 minutes or more, 90 minutes or more, 120 minutes or more, or 150 minutes or more, and may be 300 minutes or less, 270 minutes or less, 240 minutes or less, 210 minutes or less, or 180 minutes or less.

[0072] <Surface layer addition process> In the insert material preparation step, as shown in Fig. 3, a first surface layer 31 and a second surface layer 32 may be further laminated on the outside of the first outer layer 21 and the second outer layer 22. In the embodiment shown in Fig. 3, the first surface layer 31 and the second surface layer 32 are further laminated on both outsides of the insert material 100 shown in Fig. 1, but this is not limited thereto, and either the first surface layer 31 or the second surface layer 32 may be laminated. In other words, the insert material 100 may be obtained by further laminating a surface layer 30 on the outside of at least one of the first outer layer 21 and the second outer layer 22.

[0073] There are no particular limitations on the lamination method as long as the first surface layer 31 and the second surface layer 32 can be laminated without any gaps.

[0074] Examples of lamination methods include preparing plate materials and / or foil materials for the first outer layer 21, the inner layer 10, and the second outer layer 22, laminating them, and then laminating plate materials and / or foil materials for the first surface layer 31 and the second surface layer 32 on the outside. It is preferable to clean the surfaces of the plate materials and / or foil materials for each layer by degreasing and / or polishing, etc., before lamination. This makes it possible to avoid or suppress oxides and / or inclusions remaining in the joint, and as a result, it is possible to improve the joint strength.

[0075] Alternatively, the lamination method may include forming the first outer layer 21 and the second outer layer 22 on the surface of the inner layer 10, and then forming the first surface layer 31 and the second surface layer 32 on the outer side of the first outer layer 21 and the second outer layer 22. There is no particular limitation on the deposition method as long as the layers, particularly the inner layer 10, are not altered during deposition. The deposition method may include a thermal spray method, a plating method, a deposition method, etc. When the deposition method is used, it is relatively easy to laminate the layers without gaps, which leads to improved bonding strength. In addition, the layers do not separate, which is advantageous for handling the insert material.

[0076] Lamination of plate materials and / or foil materials and film formation may be combined. For example, after the first outer layer 21 and the second outer layer 22 are formed on both outer surfaces of the inner layer 10, plate materials and / or foil materials of the first surface layer 31 and the second surface layer 32 may be laminated on both outer sides.

[0077] Regarding the first surface layer 31 and the second surface layer 32, the material (composition), thickness, etc. are as explained in "<Insert Material for Liquid Phase Diffusion Bonding>".

[0078] Even when the first surface layer 31 and the second surface layer 32 are further laminated, the above-mentioned liquid phase diffusion bonding temperature, pressure, and time can be applied. In particular, the liquid phase diffusion bonding temperature is appropriately determined so that the first outer layer 21 and the second outer layer 22 undergo a eutectic reaction with the aluminum in the first aluminum member 210 and the second aluminum member 220 and is equal to or lower than the melting point of the inner layer 10. Since the first surface layer 31 and the second surface layer 32 have a lower melting point than the first outer layer 21 and the second outer layer 22, the first surface layer 31 and the second surface layer 32 melt earlier than the first outer layer 21 and the second outer layer 22 and form a liquid phase. Therefore, in the liquid phase, it is possible to avoid or suppress the bonding surfaces of the first aluminum member 210 and the second aluminum member 220 from coming into contact with the external atmosphere.

[0079] <Formate coating process, etc.> A formate coating or the like may be further formed on one or both sides of at least one of the first outer layer 21 and the second outer layer 22 to obtain the insert material 100. The formate coating "or the like" means that an acetate coating, a citrate coating, and / or a tartrate coating may be formed in addition to the formate coating. That is, one or more selected from the group consisting of a formate coating, an acetate coating, a citrate coating, and a tartrate coating may be further formed on one or both sides of at least one of the first outer layer 21 and the second outer layer 22 to obtain the insert material 100. In the following description, the coating to be formed is a formate coating, but is not limited thereto. That is, in the following description, the coating to be formed may be one or more selected from the group consisting of a formate coating, an acetate coating, a citrate coating, and a tartrate coating. In the embodiment shown in FIG. 4, the first formate coating 41 and the second formate coating 42 are formed on both sides of the first outer layer 21 and the second outer layer 22, respectively, but the present invention is not limited thereto. For example, the first formate coating 41 and the second formate coating 42 may be formed only on the outer surfaces of the first outer layer 21 and the second outer layer 22, respectively. A known method can be applied to the formation of the formate coating, and Non-Patent Document 1 can be referred to. For example, a method can be used in which the foil material for the first outer layer 21 and the foil material for the second outer layer 22 are immersed in boiled formic acid for 1 to 5 minutes, respectively, and then washed with water. By this method, the first formate coating 41 can be formed on both sides of the first outer layer 21, and the second formate coating 42 can be formed on both sides of the second outer layer 22. Then, the first outer layer 21 with the first formate coating 41, the inner layer 10, and the second outer layer 22 with the second formate coating 42 are laminated in this order, thereby obtaining the insert material 100 of the embodiment shown in FIG. 4. When forming an acetate coating, a citrate coating, or a tartrate coating, the same method can be applied, except that acetic acid, citric acid, or tartaric acid, respectively, are used instead of formic acid. The same applies to the following description.

[0080] Alternatively, the insert material 100 shown in Fig. 1 is obtained by forming the first outer layer 21 and the second outer layer 22 on both sides of a foil material for the inner layer 10 by thermal spraying or the like. The insert material 100 thus obtained is immersed in boiling formic acid for 1 to 5 minutes and then washed with water to obtain the insert material 100 provided with the first formate coating 41, the first outer layer 21, the inner layer 10, the second outer layer 22, and the second formate coating 42. That is, the first formate coating 41 and the second formate coating 42 can be formed only on one outer side of the first outer layer 21 and the second outer layer 22, respectively.

[0081] Also, for example, as shown in FIG. 5, a first surface layer 31 and a second surface layer 32 may be further laminated on the outside of the first formate coating 41 and the second formate coating .

[0082] 《Transform》 In addition to what has been described so far, the insert material and the liquid phase diffusion bonding method of the present disclosure can be modified in various ways within the scope of the claims. For example, the insert material of the present disclosure can be used in both an air atmosphere and an inert gas atmosphere. When the insert material of the present disclosure is used for liquid phase diffusion bonding in an inert gas atmosphere, the bonding strength can be further improved compared to when the insert material of the present disclosure is used for liquid phase diffusion bonding in an air atmosphere. However, even when the insert material of the present disclosure is used for liquid phase diffusion bonding in an air atmosphere, a practically acceptable bonding strength can be obtained. This is because the liquid phase derived from the first outer layer and the second outer layer can avoid or suppress the contact of the joint with the external atmosphere, and inclusions such as oxides are unlikely to remain in the joint. In particular, when the insert material of the present disclosure has a first surface layer and a second surface layer, the contact of the joint with the external atmosphere can be further avoided or suppressed. Note that the inert gas atmosphere means a gas atmosphere that is inactive against oxidation of the first aluminum member, the second aluminum member, and the insert material of the present disclosure. Such an inert gas atmosphere typically includes a nitrogen gas atmosphere in addition to an atmosphere of a gas of a Group 18 element of the long periodic table, and may be a mixed gas atmosphere of these gases and a gas of a reducing element such as hydrogen. EXAMPLES

[0083] The insert material and the liquid phase diffusion bonding method of the present disclosure will be described in more detail below with reference to examples and comparative examples. Note that the insert material and the liquid phase diffusion bonding method of the present disclosure are not limited to the conditions used in the following examples.

[0084] <Preparation of joint specimen> The joint specimens were prepared as follows.

[0085] Example 1 Foil materials for the first outer layer 21, the inner layer 10, and the second outer layer 22 were prepared. The foil materials for the first outer layer 21 and the second outer layer 22 were zinc alloy foils having a thickness of 0.6 mm. The foil material for the inner layer 10 was a metal aluminum foil having a thickness of 0.8 mm. The zinc alloy foil had a composition, by mass%, of 0.30% copper, 0.002% aluminum, 0.02% titanium, less than 0.02% lead, less than 0.01% cadmium, and less than 0.01% iron, with the remainder being zinc and unavoidable impurities.

[0086] The first outer layer 21 and the second outer layer 22 were each immersed in boiling formic acid for 2 minutes to form a first formate coating 41 and a second formate coating 42 on both sides of the first outer layer 21 and the second outer layer 22. Hereinafter, the foil material having the first formate coating 41 formed on both sides of the first outer layer 21 will be referred to as "first outer layer foil material with first formate coating" and the foil material having the second formate coating 42 formed on both sides of the first outer layer 21 will be referred to as "second outer layer foil material with second formate coating".

[0087] A first outer layer foil material with a first formate coating, an inner layer foil material, and a second outer layer foil material with a second formate coating were laminated in this order to obtain an insert material 100 of the embodiment shown in Fig. 4. That is, as shown in Fig. 4, an insert material 100 having a first formate coating 41, a first outer layer 21, a first formate coating 41, an inner layer 10, a second formate coating 42, a second outer layer 22, and a second formate coating 42 in this order was obtained.

[0088] The insert material 100 shown in FIG. 4 was sandwiched between a first aluminum member 210 and a second aluminum member 220, and the first aluminum member 210 and the second aluminum member 220 were subjected to liquid phase diffusion bonding to obtain a joint sample of Example 1.

[0089] The first aluminum member 210 was made of a Japanese Industrial Standard AC2C-T6 casting aluminum alloy, which contained, by mass%, 0.5 to 1.1% copper, 6.5 to 7.5% silicon, 0.2 to 0.4% magnesium, less than 0.1% zinc, less than 0.1% manganese, less than 0.1% nickel, and less than 0.1% tin, with the balance being aluminum and unavoidable impurities. The second aluminum member 220 was made of a Japanese Industrial Standard ADC12 die casting alloy, which contained, by mass%, 1.5 to 3.5% copper, 9.6 to 12% silicon, less than 0.3% magnesium, less than 3.0% zinc, less than 0.5% manganese, less than 0.5% nickel, and less than 0.3% tin, with the balance being aluminum and unavoidable impurities. The bonding surfaces (surfaces that come into contact with the insert material 100) of the first aluminum member 210 and the second aluminum member 220 were roughened using #1200 abrasive paper before bonding.

[0090] The liquid phase diffusion bonding conditions were as follows. Junction temperature: 400℃ Bonding pressure: 20MPa Bonding time: 15 minutes Bonding atmosphere: Air

[0091] Figure 6 shows the time variations in bonding pressure and bonding temperature during liquid phase diffusion bonding.

[0092] Example 2 A joint sample of Example 2 was prepared in the same manner as in Example 1, except that a first surface layer 31 and a second surface layer 32 were further laminated on both outer sides of the insert material used in Example 1.

[0093] In Example 2, metal tin foils having a thickness of 0.007 mm were used as the first surface layer 31 and the second surface layer 32, and these were laminated to obtain an insert material 100. That is, in Example 2, the insert material 100 shown in Fig. 5 was obtained. Specifically, the insert material 100 was obtained that includes the first surface layer 31, the first formate coating 41, the first outer layer 21, the first formate coating 41, the inner layer 10, the second formate coating 42, the second outer layer 22, the second formate coating 42, and the second surface layer 32, in this order.

[0094] Comparative Example 1 A joint sample for Comparative Example 1 was prepared in the same manner as in Example 1, except that an insert material consisting of a single layer of zinc alloy foil material with a thickness of 0.8 mm was used, and both the first aluminum member and the second aluminum member were made of AC2C-T6 cast aluminum alloy.

[0095] Comparative Example 2 A joint sample of Comparative Example 2 was prepared in the same manner as in Comparative Example 1, except that a formate coating was formed on both sides of the foil material used in Comparative Example 1. The formate coating was formed by immersing the foil material used in Comparative Example 1 in boiling formic acid for 2 minutes. "evaluation" A tensile test was performed on each of the bonded joint samples to measure the bond strength (breaking strength). The tensile direction was approximately perpendicular to the lamination surface of the insert material. The tensile speed was 10 mm / min. In addition, a scanning electron microscope was used to observe the structure of the bonded portion (as bonded) of Example 1 and Comparative Example 2. Fig. 7 is an SEM image of the bonded portion of the sample of Example 1. Fig. 8 is an SEM image of the bonded portion of the sample of Comparative Example 2.

[0096] The measurement results of the bonding strength were as follows: Comparative example 1 66.27MPa Comparative Example 2 108.05MPa Example 1 121.95 MPa Example 2 138.45 MPa

[0097] Comparing Comparative Example 1 (zinc alloy single-layer insert material without formate coating) and Comparative Example 2 (zinc alloy single-layer insert material with formate coating), the bonding strength of the sample of Comparative Example 2 is improved. This is believed to be because the oxide film on the bonding surface is removed by the formate coating. In addition, both the samples of Example 1 (see FIG. 4) and Example 2 (see FIG. 5) are provided with formate coatings on both sides of the first outer layer 21 and the second outer layer 22, and the bonding strength is even higher than that of the sample of Comparative Example 2 (zinc alloy single-layer insert material with formate coating). This is because, as shown in FIG. 8, in the sample of Comparative Example 2, the black particulate silicon phase in FIG. 8 remains in the bonding portion after agglomeration and coarsening, and it is believed that the bonding strength is reduced by this silicon phase. In contrast, as shown in FIG. 7, in the sample of Example 1, the aggregated and coarsened silicon phase does not remain in the bonding portion, and it is believed that the bonding strength is improved. This is believed to be because, in the insert material 100 of the present disclosure, the silicon phase derived from the first aluminum member 210 and the second aluminum member 220 is expelled from the joint along the inner layer 10. Also, in the insert material 100 used in Example 2 (see FIG. 5), the first surface layer 31 and the second surface layer 32 further suppressed oxidation of the joint, and it is believed that the joint strength was improved.

[0098] From the above results, the effects of the insert material for liquid phase diffusion bonding and the liquid phase diffusion bonding method of the present disclosure were confirmed. [Explanation of symbols]

[0099] 10 Inner layer 21 First outer layer 22 Second outer layer 30 Surface layer 31 First surface layer 32 Second surface layer 40 Formate Coating 41 First formate coating 42 Second Formate Coating 100 Insert material of the present disclosure 210 First aluminum member 220 Second aluminum member

Claims

1. An insert material for liquid phase diffusion bonding of a first aluminum member and a second aluminum member, at least one of which is made of an aluminum alloy containing silicon, a first outer layer, an inner layer, and a second outer layer, in that order; the first outer layer and the second outer layer are made of a metal or alloy that reacts eutectic with aluminum; the inner layer is made of a metal or alloy having a lower mass content of silicon than the aluminum alloy of at least one of the first aluminum member and the second aluminum member; the inner layer has a higher melting point than the first outer layer and the second outer layer; and the inner layer reacts eutectic with the first outer layer and the second outer layer; Insert material for liquid phase diffusion bonding.

2. 2. The insert material for liquid phase diffusion bonding according to claim 1, wherein at least one of the first outer layer and the second outer layer is made of metallic zinc or a zinc alloy.

3. 3. The insert material for liquid phase diffusion bonding according to claim 1, wherein the inner layer is made of metallic aluminum or an aluminum alloy.

4. A surface layer is further provided on the outside of at least one of the first outer layer and the second outer layer, The surface layer has a lower melting point than the first outer layer and the second outer layer, and is made of a metal or alloy that melts by itself or reacts eutectic with aluminum. The insert material for liquid phase diffusion bonding according to any one of claims 1 to 3.

5. 5. The insert material for liquid phase diffusion bonding according to claim 4, wherein the surface layer is composed of one or more selected from the group consisting of metallic tin, metallic bismuth, metallic indium, metallic gallium, a tin alloy, a bismuth alloy, an indium alloy, and a gallium alloy.

6. The insert material for liquid phase diffusion bonding according to any one of claims 1 to 5, wherein at least one of the first outer layer and the second outer layer is provided on one or both sides with one or more coatings selected from the group consisting of a formate coating, an acetate coating, a citrate coating, and a tartrate coating.

7. A method for liquid phase diffusion bonding of a first aluminum member and a second aluminum member, at least one of which is made of an aluminum alloy containing silicon, comprising: laminating a first outer layer, an inner layer, and a second outer layer in this order to obtain an insert material; disposing the insert material between the first aluminum member and the second aluminum member; and applying a load to the insert material through at least one of the first aluminum member and the second aluminum member while heating the first aluminum member, the second aluminum member, and the insert material, thereby liquid phase diffusion bonding the first aluminum member and the second aluminum member; Including, the first outer layer and the second outer layer are made of a metal or alloy that reacts eutectic with aluminum, the inner layer is made of a metal or alloy having a lower mass content of silicon than the aluminum alloy of at least one of the first aluminum member and the second aluminum member; the inner layer has a higher melting point than the first outer layer and the second outer layer; and the inner layer reacts eutectic with the first outer layer and the second outer layer; Liquid phase diffusion bonding method.

8. The transient liquid phase bonding method of claim 7 , wherein at least one of the first outer layer and the second outer layer is comprised of metallic zinc or a zinc alloy.

9. 9. The liquid phase diffusion bonding method according to claim 7 or 8, wherein the inner layer is made of metallic aluminum or an aluminum alloy.

10. Further, a surface layer is laminated on the outside of at least one of the first outer layer and the second outer layer to obtain an insert material. Including, The surface layer has a lower melting point than the first outer layer and the second outer layer, and is made of a metal or alloy that melts by itself or reacts eutectic with aluminum. The liquid phase diffusion bonding method according to any one of claims 7 to 9.

11. 11. The liquid phase diffusion bonding method according to claim 10, wherein the surface layer is made of at least one material selected from the group consisting of metallic tin, metallic bismuth, metallic indium, metallic gallium, a tin alloy, a bismuth alloy, an indium alloy, and a gallium alloy.

12. The liquid phase diffusion bonding method according to any one of claims 7 to 11, further comprising forming one or more coatings selected from the group consisting of a formate coating, an acetate coating, a citrate coating, and a tartrate coating on one or both sides of at least one of the first outer layer and the second outer layer to obtain an insert material.

Citation Information

Patent Citations

  • Joining material, manufacturing method of joining material and semiconductor device

    JP2008126272A

  • Bonding method and bonding device

    JP2012125806A

  • Method for joining metal members

    WO2016104399A1