Method for reducing odor from particulate carbon materials

A two-step process for particulate carbon materials under controlled atmospheres and temperatures effectively reduces odor emissions while maintaining material properties, addressing the odor issue in renewable-derived carbon materials.

JP7573538B2Active Publication Date: 2024-10-25SUNCOAL INDS GMBH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2021549266
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-02-21
Publication Date
2024-10-25
Estimated Expiration
2040-02-21

AI Technical Summary

Technical Problem

Particulate carbon materials, particularly those derived from renewable raw materials like lignin, emit unpleasant odors during processing, limiting their applications and requiring costly and material-intensive methods to reduce odor while preserving desired properties.

Method used

A two-step process involving precipitation and stabilization under controlled atmospheric conditions reduces odor in particulate carbon materials by minimizing oxygen exposure and controlling temperature and heating rates, maintaining desired surface area and carbon content.

Benefits of technology

The method effectively minimizes odor emissions with minimal material loss and equipment, preserving the particulate carbon materials' properties for use in elastomers, achieving reduced odor levels and improved compatibility in rubber articles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573538000008
    Figure 0007573538000008
  • Figure 0007573538000009
    Figure 0007573538000009
  • Figure 0007573538000010
    Figure 0007573538000010
Patent Text Reader

Abstract

The present invention relates to a method for reducing the odor of particulate carbon materials, and to the materials obtained thereby, as well as uses thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for reducing the odour of particulate carbon materials, and to the materials obtained thereby, as well as uses thereof. [Background technology]

[0002] Particulate carbon materials are used in many fields of application. These range from use as black dyes to use as fillers in polymers, such as elastomers, thermoplastics or thermoplastic elastomers. Such carbon-based materials can be, for example, carbon black materials with a relatively high carbon content. Other particulate carbon materials are obtained from renewable raw materials. Such particulate carbon materials have a slightly lower carbon content compared to carbon black, but show interesting properties due to the high degree of functionalization. Particularly interesting starting materials for the production of particulate carbon materials based on renewable raw materials are starting materials that can be completely or partially dissolved, such as sugars, starches or lignins. Such completely or partially dissolved starting materials based on renewable raw materials can be converted into particulate carbon materials by precipitation processes. Precipitation processes for the production of particulate carbon materials in solution are well known to the person skilled in the art.

[0003] For example, lignin-based particulate carbon materials can be produced by converting lignin dissolved in a base (e.g., sodium hydroxide solution) into acid gases (e.g., CO 2 or H 2 S) or by precipitation with acid H 2 SO 4 Examples of this prior art are given in WO 2006 / 031175, WO 2006 / 038863 or WO 2009 / 104995.

[0004] Furthermore, lignin-based particulate carbon materials can be obtained by precipitation from lignin dissolved in a base, e.g., sodium hydroxide solution, with simultaneous stabilization by increasing the temperature, e.g., to hydrothermal carbonization conditions. Examples of this prior art are described in WO 2016 / 020383 or WO 2017 / 085278. The methods of precipitation by introduction of acid gas, by addition of acid or by increasing temperature can also be combined.

[0005] In the production of particulate carbon materials, the adaptation of certain process parameters opens up the possibility in particular of influencing the particle size to be obtained (i.e. the size of the agglomerates to be obtained, composed of primary particles), as well as the setting of surface parameters, in particular the specific surface area, which is also used as a measure of the primary particle size. The same can be quantified, for example, by methods of measuring the surface area, such as BET or STSA measurements. In this case, BET measurements determine the sum of the external and internal surfaces, while STSA measurements solely determine the external surface. Suitable measurement methods are given, for example, in ASTM D 6556-14.

[0006] It is known that the average size or specific surface area of ​​the primary particles influences the properties of materials produced by using particulate carbon materials, for example rubber articles produced by compounding particulate carbon materials with elastomers and subsequent crosslinking. For example, the wear behavior of rubber articles differs depending on whether particulate carbon materials with higher or lower BET surface areas are used. A similar situation exists for mechanical properties such as tensile strength. High values ​​of BET surface area correlate with high tensile strength values ​​and low wear. Here, when using particulate carbon materials, it is necessary to have a specific surface area of ​​at least 5 m to obtain high quality rubber articles. 2 / g, preferably at least 8m 2 / g, more preferably at least 10m 2 / g, more preferably at least 15m 2 / g or more is often required.

[0007] However, a drawback of known particulate carbon materials, for example obtained by precipitation of totally or partially dissolved starting materials based on renewable raw materials, in particular lignin-based particulate carbon materials, is the unpleasant odor emanating from the particulate carbon material itself, released during the processing of the particulate carbon material and / or emanating from materials containing the particulate carbon material, which severely limits the potential applications of very interesting particulate carbon materials.

[0008] Methods for reducing the odor of lignin-based particulate carbon materials are known in the prior art. These rely on the one hand, for example, on extraction methods (WO 2013 / 101397), enzyme-catalyzed reactions (DE 10 2006 057566), prepurification of lignin by treatment with oxidizing components followed by washing (DE 10 1013 001678), and on the other hand, for example, on the treatment of black liquor, evaporation processes, treatment with reducing or oxidizing agents, or prepurification of lignin by chlorination reactions and high-temperature treatment. However, such methods require the treatment of relatively large amounts of material or the use of chemicals, which is disadvantageous both in terms of the amount of equipment and financial expenditure.

[0009] It is therefore desirable to provide a method that allows targeted reduction of odors emitted from particulate carbon materials, such as those emitted during processing of the particulate carbon materials and / or from materials containing the particulate carbon materials, preferably by processing of already obtained particulate carbon materials, without using additional process chemicals. In this way, costs and the amount of equipment can be reduced, while at the same time smaller amounts of material are processed. However, another requirement of such a method is that the desired properties of the particulate carbon materials, such as the specific surface area, are not lost during the odor reduction treatment.

[0010] Furthermore, since particulate carbon material is already a valuable product, material losses cannot be too high. Summary of the Invention [Problem to be solved by the invention]

[0011] It is therefore an object of the present invention to indicate such a method for providing the above-mentioned particulate carbon material. [Means for solving the problem]

[0012] This object is achieved by a method as defined in claim 1 and a product as defined in claim 7, as well as by a use as defined in claim 10. Preferred embodiments and further aspects of the invention result from the further claims and the embodiments given in the detailed description below. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 shows a schematic diagram of a possible temperature profile for one example of a method according to the invention. [Diagram 2] FIG. 2 shows the BET surface area of ​​starting materials and heat-treated particulate carbon materials of the present invention as a function of the maximum temperature reached during processing. [Diagram 3-4] FIG. 1 shows the surface quality of a pressure-free vulcanized elastomer compound made with particulate carbon material before and after carrying out the method of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The method of the present invention allows for facile odor reduction of particulate carbon materials produced from starting materials based on renewable raw materials.

[0015] For example, the method according to the invention is characterized in that in a first process step a particulate carbon material (hereinafter pKM) is obtained, the odor of which is reduced in a second process step, thereby obtaining a reduced odor pKM. This pKM can be, for example, precipitated lignin, but pKM is preferred, in particular one based on lignin that has additionally been subjected to hydrothermal carbonization.

[0016] Preferably, all or part of the starting material is soluble in a liquid, more preferably the starting material consists of more than 50% sugar, starch or lignin.

[0017] In the following, a preferred embodiment of the first process step is described: in the present invention, it is not important whether this first process step is performed immediately before the second process step or whether this first step is performed significantly prior to the second step in terms of time (so, for example, pKM from the first step is generated separately and then stored before being subjected to the second step).

[0018] Preferably, the pKm is obtained in a first process step by precipitation of a fully or partially dissolved starting material. If the starting material consists of more than 50% lignin, the pKM is preferably obtained by precipitation of a fully or partially dissolved lignin in a liquid by introduction of an acid gas and / or by addition of an acid and / or by precipitation and simultaneous stabilization under hydrothermal carbonization (HTC) conditions. Such methods are known to the skilled person and are described in WO 2006 / 031175 or WO 2006 / 038863 or WO 2009 / 104995 (precipitation) or WO 2016 / 020383 or WO 2017 / 085278 (precipitation and co-stabilization). After the first process step, the pKM is at least 5 m 2 / g, preferably at least 8m 2 / g, more preferably at least 10m 2 / g, more preferably at least 15m 2 It has proven advantageous to have a BET surface area of ​​at least 200 m / g. Advantageously, the BET surface area is 2 / g or less, preferably 180m 2 / g or less.

[0019] Advantageously, the BET surface area of ​​the pKM deviates from its STSA surface area by at most 20%, preferably at most 15%, more preferably at most 10%. It is therefore preferred that the pKM is not porous.

[0020] In addition, pKM preferably exhibits a carbon content (based on ash-free dry matter) of 50 to 80% by weight (wt%), more preferably 60 to less than 80% by weight. pKM is therefore a different raw material from carbon black by its carbon content. As pKM is preferably produced by precipitation or precipitation combined with stabilization (e.g. HTC), the lower carbon content compared to carbon black at the same time ensures that a high content of functional groups is present on the particles. This can be advantageous for the subsequent use of pKM.

[0021] A preferred embodiment of the second process step is further described below: According to the invention, the pKM is converted in a second process step into an odor-reducing pKM in a gas atmosphere.

[0022] Advantageously, the second process step is carried out under a process atmosphere rather than under air.

[0023] The process atmosphere may be, for example: - air enriched by means of an inert gas having an oxygen content of less than 15% by volume, preferably less than 10% by volume, more preferably less than 5% by volume and particularly preferably less than 3% by volume, and / or - understood to mean reduced pressure air having a pressure of less than 500 mbar, preferably less than 200 mbar and more preferably less than 100 mbar.

[0024] Advantageously, the treatment atmosphere, consisting of air enriched with an inert gas, has an oxygen content of at least 0.1% by volume, preferably at least 0.5% by volume and particularly preferably at least 1% by volume.

[0025] Suitable inert gases in the sense of the present invention are in particular nitrogen, carbon dioxide, superheated steam or gases released from the pKM during the second process step. Gases released from the pKM during the second process step also include, for example, carbon monoxide, hydrogen, etc., but are referred to herein as inert gases. The pressure can be selected according to the possibilities or requirements of using air enriched with inert gas as the process atmosphere, as already mentioned above. In terms of equipment, it is easiest to carry out the process at ambient pressure or simply at a slightly negative or excess pressure, for example ±10 mbar.

[0026] The second process step is preferably controlled (e.g. by selecting the temperature profile, the maximum temperature, the process atmosphere, optionally by selecting the pressure) so that the mass loss of the pKM in the second process step is less than 20%, preferably less than 15%, more preferably less than 10%. In order to reduce the odorous substance content, a certain mass loss is required during the second process step of the method according to the invention. This mass loss is usually at least 1% or more, preferably at least 2% or more, possibly even 5% or more. This ensures and achieves that not too much material is lost, while the desired odor reduction is achieved. The suitability of the treated pKM for use, for example as a filler in elastomers, can then also be guaranteed.

[0027] Regardless of the choice of the process atmosphere of the second process step, the process temperature in the second process step should exceed a minimum temperature and should not exceed a maximum temperature. The maximum temperature is 300°C, preferably not more than 250°C, more preferably not more than 230°C. The minimum temperature is 150°C, preferably 160°C, more preferably 170°C, and in some cases 180°C. The holding time during which the pKM is held in the process atmosphere at the process temperature in the second process step can be selected over a wide range. Suitable values ​​are ≥ 1 second and ≤ 5 hours. Preferably, the holding time is ≤ 60 minutes, more preferably ≤ 30 minutes, most preferably ≤ 15 minutes, and in some cases less than 10 minutes.

[0028] Preferably the process temperature of the second process step is not more than 50°C, preferably not more than 40°C, more preferably not more than 30°C, particularly preferably not more than 20°C, in particular not more than 10°C, and is selected to be higher than the further processing and / or utilization temperatures, but not below a minimum temperature and not above a maximum temperature.

[0029] Preferably, the process temperature of the second process step is selected to be at least 50° C., preferably at least 40° C., more preferably at least 30° C., particularly preferably at least 20° C., in particular at least 10° C. lower than the further processing and / or utilization temperature.

[0030] Further processing temperature means the temperature at which the odor reducing pKM is further processed into a product when mixed with other materials. For example, if the odor reducing pKM is incorporated into a rubber compound, the further processing temperature means, for example, the temperature at which the rubber compound is crosslinked, for example, between 150°C and 180°C if sulfur crosslinking is used.

[0031] By application temperature is meant the temperature at which a product containing the odor-reducing pKM is used. For example, if the odor-reducing pKM is used in an EPDM-based product, the application temperature may be, for example, 150° C. or less. For example, if the odor-reducing pKM is used in an FKM-based product, the application temperature may be, for example, 250° C. or less.

[0032] If the further processing temperature and / or application temperature is lower than the temperature of the first processing step, the processing temperature preferably does not exceed, is more preferably lower, particularly preferably at least 1°C lower, even more preferably at least 5°C lower than the temperature of the first processing step.

[0033] In a preferred embodiment, the stabilization of the lignin-based starting material in the first process step is carried out under hydrothermal carbonization conditions, and in the second process step, the temperature of stabilization under hydrothermal carbonization conditions is preferably not exceeded, more preferably not reached, particularly preferably reduced to at least 1°C, more preferably reduced to at least 5°C.

[0034] It has proven advantageous that in the second process step the pKM is treated under the process atmosphere not only during the holding time, but also the heating and cooling takes place under the process atmosphere.

[0035] An essential point for improving the second process step is the combination of heating rate and process temperature. On the other hand, the cooling rate can be chosen freely. Preferably, the heating of the pKM to a process temperature above the critical temperature is only carried out in a controlled manner. Until the critical temperature is reached, the heating rate can be chosen freely (i.e. here, for example, the heating can be very fast). However, from the critical temperature, control of the heating rate is important. It has been shown that uncontrolled heating above the critical temperature leads to disadvantageous effects, in particular undesirable high mass losses and large losses of BET surface area. Heating rates below 30 ° C / min from the critical temperature, in particular below 20 ° C / min, have been found to be particularly advantageous. The preferred range of heating rates is in the range from 1 ° C / min to 20 ° C / min, such as from 5 ° C / min to 10 ° C / min. If the maximum temperature of the treatment is 250 ° C or higher, it has been found to be preferred if the heating rate is particularly low in this temperature range, for example from 0.1 ° C / min to 5 ° C / min.

[0036] The critical temperature depends on which starting material is converted to pKM in the first process step and how the first process step is designed. The critical temperature is usually between 80°C and 250°C, more preferably between 100°C and 230°C. When pKM is obtained in a first process step from softwood lignin, for example by precipitation with complex stabilization under hydrothermal carbonization conditions, the critical temperature in the second process step is preferably between 150°C and 230°C, more preferably between 180°C and 220°C.

[0037] If the pKM in the first process step is obtained from hardwood lignin, for example by precipitation combined with complex stabilization under hydrothermal carbonization conditions, the critical temperature in the second process step is preferably between 130°C and 200°C, more preferably between 140°C and 180°C.

[0038] If pKM is obtained in a first process step from softwood lignin, for example by precipitation combined with stabilization under hydrothermal carbonization conditions, then in a second process step, for example at a maximum treatment temperature of 250° C. or less, about 5 m 2 A loss of BET surface area of ​​less than 10% can be achieved at the same time (i.e., when the pKM is less than 40m 2 / g, it has a maximum BET surface area of ​​35m 2 / g). At the same time, odor testing showed a significant reduction in unpleasant odors, which was found during the manufacture of rubber articles filled with the reduced odor pKM, as well as for rubber articles compared to those having a pKM that had not been subjected to the second process step (e.g., found for the reduced odor pKM).

[0039] Thus, the method according to the invention can achieve a good balance between the desired odor minimization and the simultaneous extensive preservation of the desired material properties and low mass loss. Neither the use of process chemicals nor complicated methods are necessary. Also, the maximum temperature of the treatment according to the invention is in a relatively low range, which is advantageous both in terms of cost and process control.

[0040] The equipment used to carry out such treatment is well known to those skilled in the art.Preferably, the second process step is carried out in a rotary kiln or in a fluidized bed.More preferably, the second process step can be combined with grinding or classification (for example, gas jet mill, turbo rotor mill or air classifier).

[0041] As already mentioned above, the pKM obtained according to the invention is preferably obtained on the basis of lignin, preferably obtained by precipitation or precipitation by combined stabilization, for example under hydrothermal carbonization conditions, which pKM is proposed for use in rubber compounds. In the present invention, it has been shown that the odor-reduced pKM produced according to the invention is particularly suitable for use in elastomeric compounds in which the desired rubber article is produced by pressureless vulcanization. Here, rubber articles containing pKM produced according to the prior art not only show odor development during vulcanization and odor of the obtained vulcanizate, but also undesirable porosity, which significantly reduces the mechanical properties. Here, the method according to the invention makes it possible to overcome this drawback. The odor development can possibly be reduced to an acceptable level by a limited period of storage after the production of the product, but in principle is unacceptable in products affected by porosity. This can even be avoided in the context of the present invention.

[0042] In the present invention, the odor-reducing pKMs produced according to the present invention have also been modified with respect to polarity or hydrophobicity, and have also been shown to be, for example, more suitable for use in hydrophobic or less polar elastomeric compounds than pKMs produced according to the prior art.

[0043] Advantageously, an odour-reduced particulate carbon material is obtained by the method described above.The present invention therefore also provides an odour-reduced pKM, preferably obtainable by the method according to the invention.

[0044] Odor reducing pKMs differ from prior art materials in, for example, the following ways: - Minimum 5m 2 / g BET, - The odor of a rubber article produced using 50 phr of the odor-reduced pKM is more comparable to the odor of a rubber article produced using 50 phr of N550 than to the odor of a rubber article produced using 50 phr of lignoboosted lignin.

[0045] Preferably, the odor reducing pKM has a dimethylsulfide content of 1 mg / kg or less, preferably 0.5 mg / kg or less, more preferably less than 0.1 mg / kg, even more preferably less than 0.05 mg / kg, especially less than 0.01 mg / kg.

[0046] Preferably the odour reducing pKM has a guaiacol content of 0.1 mg / kg or less, preferably 0.05 mg / kg or less, more preferably less than 0.01 mg / kg, even more preferably less than 0.005 mg / kg, especially less than 0.001 mg / kg.

[0047] Preferably, the odor reducing pKM has a naphthalene content of less than 5 mg / kg (DIN EN 16181:2017-11 / draft). Preferably, the sum of the 18 EPA-PAKs excluding BG (DIN EN 16181:2017-11 / draft) is less than 5 mg / kg. Preferably, the content of benzo(a)anthracene, chrysene, benzo(b)fluoroanthene, benzo(k)fluoroanthene, benzo(a)pyrene, indenol(1,2,3-cd)pyrene, dibenzol(a,h)anthracene, benzene(ghi)perylene, benzo(e)pyrene and benzo(j)fluoroanthene is undetectable (<0.1 mg / kg) (DIN EN 16181:2017-11 / draft).

[0048] Odor reducing pKMs differ, for example, from prior art materials in the following ways: - 5m 2 / g or more BET, - The porosity of rubber articles produced by pressureless vulcanization using 50 phr of odor reduced pKM is comparable to the porosity of rubber articles produced by pressureless vulcanization using 50 phr of N550 compared to the porosity of rubber articles produced by pressureless vulcanization using 50 phr of lignoboosted lignin.

[0049] For example, odor reducing pKMs differ from prior art materials in that: - Minimum 5m 2 / g BET, - The Klason lignin content is at least 90%; the proportion of substances associated with unpleasant odors, such as dimethyl disulfide, measured by HS-GC / MS at 160° C., is reduced to less than 30%, preferably less than 25%. EXAMPLES

[0050] Example 1 1st step: pKM (raw material A) was obtained from softwood lignin by stabilization under hydrothermal carbonization conditions. Second step: 40m 2 10 kg of feedstock A with a BET of 1000 / g (measured according to ASTM D 6556-14) was treated in a drying cabinet at 250° C. for 3 hours. The oxygen content in the drying cabinet was reduced to less than 10% by volume during heating, the holding time and cooling by rinsing with nitrogen. The heating rate was 1 K / min from a temperature of 150° C. 2 9.6 kg of odor reducing pKM (Feedstock B) was obtained having a BET of 1.0 g / g. Feed A and Feed B were analyzed by headspace GC / MS at 160° C. The following results were obtained:

[0051] [Table 1]

[0052] Feeds A and B do not differ significantly in their elemental sulfur content, despite the drop in sulfur-containing compounds. The elemental composition is simply an increase in the carbon content of Feed B, which was treated according to the method of the present invention. Feed B also showed a 9% increase in fixed carbon content.

[0053] [Table 2]

[0054] Example 2 40m 2 Feedstock A from Example 1 with BET of 30m 2 / g BET (odor reducing pKM), and 30m 2 A third pKM (Feedstock C) having a BET of 1.0001 / g was blended as a filler into the SBR matrix. After vulcanization, the stress-strain curve progression was recorded in a tensile test. The tensile strength results are shown in Table y.

[0055] [Table 3]

[0056] The preparation of the mixture into an elastomeric compound and the preparation of the vulcanizate were carried out according to the following recipe by the following means:

[0057] [Table 4]

[0058] The mixtures were prepared by the following method: The mixtures were prepared at 70% fullness using a Haake Rheomix 3000 measuring mixer (tangential rotor geometry). The mixing temperature was kept constant by speed control. The mixing time was about 20 min. The vulcanization was carried out at 160°C according to the optimum t90 time determined by the rheometer + 1 min per mm of plate thickness.

[0059] Example 3: 40m2 Raw material A from Example 1 having a BET of 30m 2 Raw material B (odor reducing pKM) from Example 1 having a BET of 100 / g was blended as a filler into the EPDM matrix. After vulcanization, the course of the stress-strain curve was recorded in a tensile test. The results are shown in Table x:

[0060] [Table 5]

[0061] [Table 6]

[0062] The mixtures were prepared by the following method: The mixture was prepared using a W&P Type GK1.5E mixer (intermesh rotor configuration) at a fill level of 70%, mixer temperature of 40° C., and speed of 40 rpm.

[0063] Vulcanization was carried out by baking at 160°C according to the optimum t90 time determined by rheometer.

[0064] For pressureless vulcanization, two test specimens were prepared from 6 mm thick compound skins using a volumetric die cutter and vulcanized in a heating cabinet for 30 min at 160° C. After collection, one specimen was immediately cut open and evaluated for odor and porosity, and the second specimen was cut open and evaluated after cooling to room temperature. Since in-process pressureless vulcanization the material typically undergoes an extrusion process in which it is exposed to pressure in a die that removes most of the entrapped air, it can be assumed that the actual in-process porosity is even lower than that determined by this laboratory method. The rubber articles made with Ingredient A had the following porosities: The rubber articles made with Stock B had the following porosities:

[0065] Example 4 1st step: pKM (raw material D) was obtained from softwood lignin by stabilization under hydrothermal carbonization conditions.

[0066] Second step: 31.1m 2 Feedstock D, with a BET of 10000 / g, was subjected to the method at various temperatures. Nitrogen was selected as the process atmosphere. Feedstock D was treated at the heat treatment temperatures shown in the table. Heating was performed without heating rate control (naturally) or with a heating rate of 10 K / 10 min from the critical temperature of 150° C. (150 to 10 K / 10 min). Additionally, the BET of the odor reducing pKM is shown.

[0067] [Table 7]

[0068] This example shows that a temperature increase without heating rate control can be achieved up to a heat treatment temperature of 200° C. without significantly affecting the BET. This example further shows that a temperature increase with heating rate control can be carried out from the critical temperature of 150° C. to a temperature of 400° C. without significantly affecting the BET.

Claims

1. A method for producing a particulate carbon material having reduced odor, comprising the steps of: The starting material contains more than 50% lignin. a first process step in which a particulate carbonaceous material is prepared by precipitation of the starting material, fully or partially dissolved in a liquid, by introduction of an acidic gas and / or addition of an acid; the particulate carbon material is subsequently treated in a second process step by heating in a gas atmosphere to obtain an odor-reducing particulate carbon material; In the second process step, the process temperature is such that the maximum temperature does not exceed 300° C. and the minimum temperature does not fall below 150° C.; The gas atmosphere in the second process step is a) air enriched with an inert gas having an oxygen content of less than 15% by volume, and / or b) reduced pressure air, having a pressure of less than 500 mbar; A method selected from the group consisting of

2. 2. The method according to claim 1, wherein the oxygen content of the gas atmosphere consisting of air enriched with an inert gas is at least 0.1% by volume.

3. The particulate carbon material is at least 5 m after the first process step. 2 / g or more 200m 2 3. The method of claim 1 or 2, wherein the SiO2 has a BET surface area of ​​0.1 to 1.0 g / g or less.

4. A method according to any one of claims 1 to 3, wherein during the second process step the process temperature in the gas atmosphere of particulate carbon material is maintained for at least 1 second and less than 60 minutes.

5. A method according to any one of claims 1 to 4, wherein in the second process step the particulate carbon material is treated in a gas atmosphere at the process temperature and further heated and cooled in said gas atmosphere.

6. The method according to any one of claims 1 to 5, wherein the second process step is carried out in a rotary kiln or in a fluidized bed.

7. The method according to any one of claims 1 to 6, wherein the second process step is performed in combination with grinding or classification.

8. 8. The method according to any one of claims 1 to 7, wherein the inert gas is selected from the group consisting of nitrogen, carbon dioxide, superheated steam and the gas released during the second process step, and / or air having an oxygen concentration of less than 10% by volume enriched with an inert gas.

9. 9. The method of any one of claims 1 to 8, wherein the odor-reduced particulate carbon material has a dimethylsulfide and guaiacol content of less than 1 mg / kg.

10. 10. The method of claim 1, wherein the odor-reduced particulate carbon material has a naphthalene content of less than 5 mg / kg.

11. The method according to any one of claims 1 to 10, wherein the particulate carbon material having reduced odor has a content of 18 EPA-PAK excluding BG (according to DIN EN16181:2017-11 / draft) of less than 5 mg / kg.

12. The method according to any one of claims 1 to 10, wherein the odor-reduced particulate carbon material has a content of benzo(a)anthracene, chrysene, benzo(b)fluoroanthene, benzo(k)fluoroanthene, benzo(a)pyrene, indenol(1,2,3-cd)pyrene, dibenzol(a,h)anthracene, benzene(g,h,i)perylene, benzo(e)pyrene and benzo(j)fluoroanthene of less than 0.1 mg / kg.

13. Use of a particulate carbon material having reduced odor obtainable by the method according to any one of claims 1 to 12 as an additive in polymer blends, in particular elastomer blends.

14. Odor-reduced fine carbon particles a) A BET surface area of ​​at least 5 m 2 / g, b) Dimethyl sulfide and guaiacol content less than 1 mg / kg; c) BET surface area with a maximum deviation of 20% from the STSA surface area; d) a carbon content of 50 to 80% by mass, based on ash-free dry matter; e) the content of benzo(a)anthracene, chrysene, benzo(b)fluoroanthene, benzo(k)fluoroanthene, benzo(a)pyrene, indenol(1,2,3-cd)pyrene, dibenzol(a,h)anthracene, benzene(g,h,i)perylene, benzo(e)pyrene and benzo(j)fluoroanthene is less than 0.1 mg / kg; The method according to any one of claims 1 to 12.

Citation Information

Patent Citations

  • Thermoplastic lignin for carbon fiber manufacturing

    JP2013542276A

  • Particulate carbon material that can be produced from renewable raw materials and method for producing the same