Sensor element and gas sensor
The sensor element addresses stress and crack issues by optimizing heating element positioning and resistance ratios, enhancing stress reduction and detection accuracy in gas sensors.
Patent Information
- Application Number
- JP2022125362
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-08-25
- Filing Date
- 2022-08-05
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2042-08-05
AI Technical Summary
Conventional gas sensors experience stress generation around the internal space due to heating, which can lead to cracks, and existing solutions do not adequately address this issue.
The sensor element design includes a heating element with specific positional relationships and overlapping areas to reduce stress, ensuring distances X1 and X2 satisfy certain ratios relative to the pump chamber widths, and maintains a unit resistance value ratio R3/R1 less than 1 to prevent temperature differences affecting detection accuracy.
This design effectively reduces stress around internal spaces and maintains detection accuracy by ensuring sufficient heating of pump cells while minimizing crack occurrence and temperature disparities.
Smart Images

Figure 0007573575000002 
Figure 0007573575000003 
Figure 0007573575000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a sensor element and a gas sensor. [Background technology]
[0002] Conventionally, a sensor element used in a gas sensor for detecting a specific gas concentration such as NOx in a measurement gas such as an automobile exhaust gas has been known. For example, Patent Document 1 describes a sensor element including a laminate of a plurality of oxygen ion conductive solid electrolyte layers, an internal space provided inside the laminate, a pump cell for pumping oxygen in and out of the internal space, and a measurement electrode disposed inside the laminate. When detecting the concentration of NOx with this sensor element, first, the oxygen concentration of the measurement gas in the internal space is adjusted. Next, the NOx in the measurement gas after the oxygen concentration is adjusted is reduced around the measurement electrode. Then, the concentration of NOx in the measurement gas is detected based on the pump current that flows when the oxygen around the measurement electrode is pumped out. In addition, the sensor element of Patent Document 1 includes a heating element that plays a role of temperature adjustment for heating and keeping the sensor element warm in order to increase the oxygen ion conductivity of the solid electrolyte. This heating element has a straight portion and a bent portion. The bent portion has a lower resistance per unit length than the straight portion at least at any temperature in the temperature range of 700° C. to 900° C. This makes it difficult to increase the temperature of the bent portion, which is more susceptible to deterioration than the straight portion, and thus makes it possible to suppress deterioration of the bent portion. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-041431 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, when the heating element heats the sensor element, stress may be generated around the internal space of the sensor element. This stress may cause cracks in the sensor element, so it is desirable to reduce the stress. Patent Document 1 does not take into account the stress generated around the internal space.
[0005] The present invention has been made to solve the above problems, and has as its main object to reduce the stress that occurs around the internal space of the sensor element when the heating element generates heat. [Means for solving the problem]
[0006] In order to achieve the above-mentioned main object, the present invention adopts the following means.
[0007] [1] The sensor element of the present invention comprises: a plate-shaped element body including an oxygen ion conductive solid electrolyte layer, a measurement gas flow section for introducing and flowing a measurement gas therein, and having a longitudinal direction, a lateral direction, and a thickness direction perpendicular to the longitudinal direction and the lateral direction; a main pump cell for adjusting the oxygen concentration in a main pump chamber of the measurement gas flow section; an auxiliary pump cell that adjusts the oxygen concentration in an auxiliary pump chamber that is provided downstream of the main pump chamber in the measurement gas flow portion; a measurement pump cell for adjusting an oxygen concentration in a measurement chamber provided downstream of the auxiliary pump chamber in the measurement gas flow portion; A heating element for heating the element body; Equipped with The heating element is A first outer straight portion and a second outer straight portion are aligned along the short side direction and have a length direction along the longitudinal direction; a first inner straight line portion and a second inner straight line portion that are disposed between the first outer straight line portion and the second outer straight line portion in the short side direction and whose length direction is aligned with the longitudinal direction; a first bent portion connecting the first outer straight portion and the first inner straight portion at one end side in the longitudinal direction; a second bent portion connecting the first inner straight portion and the second inner straight portion at the other end side in the longitudinal direction; a third bent portion connecting the second inner straight portion and the second outer straight portion at one end side in the longitudinal direction; having the first inner straight portion and the second inner straight portion each at least partially overlap a main pump chamber projection area, which is an area obtained by projecting the main pump chamber in the thickness direction toward the heat generating element; the first inner straight portion and the second inner straight portion each at least partially overlap with an auxiliary pump chamber projection area, which is an area obtained by projecting the auxiliary pump chamber toward the heating element in the thickness direction; a distance X1 between the first inner straight portion and the second inner straight portion in the short side direction at a portion where the first inner straight portion and the second inner straight portion overlap with the main pump chamber projection area is equal to or greater than 1 / 3 of a width Wp in the short side direction of the main pump chamber projection area, The first inner straight portion and the second inner straight portion have a mutual distance X2 in the short side direction at a portion overlapping with the auxiliary pump chamber projected area, the mutual distance X2 being 0.4 times or more of the width Wp. It is something.
[0008] In this sensor element, the positional relationship between the heating element and the internal space of the sensor element (main pump chamber, auxiliary pump chamber, and measurement chamber) satisfies the condition that the distance X1 is 1 / 3 or more of the width Wp, and the distance X2 is 0.4 times or more of the width Wp. The distance X1 is the short-side distance between the first inner straight portion and the second inner straight portion of the heating element at the portions overlapping with the main pump chamber projection area, which is the area where the main pump chamber is projected in the thickness direction toward the heating element. The distance X2 is the short-side distance between the first inner straight portion and the second inner straight portion of the heating element at the portions overlapping with the auxiliary pump chamber projection area, which is the area where the auxiliary pump chamber is projected in the thickness direction toward the heating element. The width Wp is the short-side length of the main pump chamber projection area. By satisfying the above conditions, it is possible to reduce stress generated around the internal space (main pump chamber, auxiliary pump chamber, and measurement chamber) when the heating element generates heat.
[0009] [2] In the sensor element described above (the sensor element described in [1] above), the distance X1 may be greater than 0.4 times the width Wp. This enhances the effect of reducing the stress described above.
[0010] [3] In the sensor element described above (the sensor element described in [1] or [2] above), the resistance per unit length of the pump chamber overlapping portion, which is a portion of the heating element overlapping with a pump chamber projection area, which is a region of the main pump chamber and the auxiliary pump chamber projected toward the heating element in the thickness direction, is defined as unit resistance R1 [μΩ / mm], and the resistance per unit length of the measurement chamber overlapping portion, which is a portion of the heating element overlapping with a measurement chamber projection area, which is a region of the measurement chamber projected toward the heating element in the thickness direction, is defined as unit resistance R3 [μΩ / mm]. In this case, the unit resistance ratio R3 / R1 may be less than 1 at least at any temperature in a temperature range of 700°C to 900°C. Here, if the unit resistance R3 is too large, the difference between the temperature around the main pump chamber and the auxiliary pump chamber and the temperature around the measurement chamber becomes too small, which may result in a decrease in the detection accuracy of the specific gas concentration. By having the unit resistance ratio R3 / R1 be less than 1, such a decrease in detection accuracy can be suppressed.
[0011] In this case, the measurement chamber overlapping portion may be at least a part of the second bent portion. In other words, the second bent portion of the heating element may overlap with the measurement chamber projection area.
[0012] [4] A gas sensor according to the present invention includes the sensor element according to any one of the above [1] to [3]. Therefore, the gas sensor can obtain the same effects as the sensor element according to the present invention described above, for example, the effect of reducing stress generated around the internal space of the sensor element when the heating body generates heat. [Brief description of the drawings]
[0013] [Figure 1] 1 is a schematic cross-sectional view illustrating an example of the configuration of a gas sensor 100. FIG. [Diagram 2] Cross section AA of Figure 1. [Diagram 3] FIG. 13 is an explanatory diagram of a heater 72 according to a modified example. [Figure 4] FIG. 13 is an explanatory diagram of a heater 72 according to a modified example. [Diagram 5] Graph plotting the results of stress evaluation of distances X1, X2, and internal voids in Experimental Examples 1 to 9. [Figure 6] 1 is a graph plotting the results of stress evaluation of distances X1, X2, and the outer periphery for Experimental Examples 1 to 9. [Figure 7] FIG. 13 is an explanatory diagram of a heater 72 in Experimental Example 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Next, an embodiment of the present invention will be described with reference to the drawings. FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a gas sensor 100 according to an embodiment of the present invention. FIG. 2 is a cross-sectional view taken along line AA in FIG. 1. The gas sensor 100 detects the concentration of a specific gas, such as NOx, in a measurement gas, such as an automobile exhaust gas, by a sensor element 101. The sensor element 101 has a long rectangular parallelepiped shape, and the longitudinal direction of the sensor element 101 (the left-right direction in FIG. 1) is defined as the front-rear direction, and the thickness direction of the sensor element 101 (the up-down direction in FIG. 1) is defined as the up-down direction. The width direction of the sensor element 101 (the direction perpendicular to the front-rear direction and the up-down direction) is defined as the left-right direction.
[0015] The sensor element 101 is an element having a laminate in which six layers, namely a first substrate layer 1, a second substrate layer 2, a third substrate layer 3, a first solid electrolyte layer 4, a spacer layer 5, and a second solid electrolyte layer 6, each of which is made of an oxygen ion conductive solid electrolyte layer such as zirconia (ZrO2), are laminated in this order from the bottom as viewed in the drawing. The solid electrolyte forming these six layers is dense and airtight. The sensor element 101 is manufactured, for example, by performing a predetermined processing and printing a circuit pattern on ceramic green sheets corresponding to each layer, laminating them, and further firing them to integrate them.
[0016] At the front end side (the left end side in FIG. 1) of the sensor element 101, between the lower surface of the second solid electrolyte layer 6 and the upper surface of the first solid electrolyte layer 4, a gas inlet 10, a first diffusion rate-controlling section 11, a buffer space 12, a second diffusion rate-controlling section 13, a first internal void 20, a third diffusion rate-controlling section 30, a second internal void 40, a fourth diffusion rate-controlling section 60, and a third internal void 61 are formed adjacent to each other and communicated with each other in this order.
[0017] The gas inlet 10, the buffer space 12, the first internal void 20, the second internal void 40, and the third internal void 61 are spaces inside the sensor element 101, which are defined by an upper portion cut out of the spacer layer 5, the lower portion cut out by the upper surface of the first solid electrolyte layer 4, and the sides cut out by the side surfaces of the spacer layer 5.
[0018] The first diffusion rate-controlling section 11, the second diffusion rate-controlling section 13, and the third diffusion rate-controlling section 30 are each provided as two horizontally elongated slits (with the opening extending in the direction perpendicular to the drawing). The fourth diffusion rate-controlling section 60 is provided as one horizontally elongated slit (with the opening extending in the direction perpendicular to the drawing) formed as a gap with the lower surface of the second solid electrolyte layer 6. The portion from the gas inlet 10 to the third internal space 61 is also referred to as a measurement gas flow section.
[0019] Further, at a position farther from the tip side than the measurement gas flow portion, a reference gas introduction space 43 is provided between the upper surface of the third substrate layer 3 and the lower surface of the spacer layer 5, and at a position defined at the side by the side surface of the first solid electrolyte layer 4. For example, air is introduced into the reference gas introduction space 43 as a reference gas when measuring the NOx concentration.
[0020] The air introduction layer 48 is a layer made of porous ceramics, and a reference gas is introduced into the air introduction layer 48 through the reference gas introduction space 43. The air introduction layer 48 is formed so as to cover the reference electrode 42.
[0021] The reference electrode 42 is an electrode formed in a manner to be sandwiched between the upper surface of the third substrate layer 3 and the first solid electrolyte layer 4, and as described above, is surrounded by an air introduction layer 48 connected to a reference gas introduction space 43. As will be described later, the reference electrode 42 can be used to measure the oxygen concentration (oxygen partial pressure) in the first internal space 20, the second internal space 40, and the third internal space 61. The reference electrode 42 is formed as a porous cermet electrode (for example, a cermet electrode of Pt and ZrO2).
[0022] In the measurement gas flow section, the gas inlet 10 is a section that opens to the external space, and the measurement gas is introduced into the sensor element 101 from the external space through the gas inlet 10. The first diffusion rate-controlling section 11 is a section that imparts a predetermined diffusion resistance to the measurement gas introduced from the gas inlet 10. The buffer space 12 is a space provided for guiding the measurement gas introduced from the first diffusion rate-controlling section 11 to the second diffusion rate-controlling section 13. The second diffusion rate-controlling section 13 is a section that imparts a predetermined diffusion resistance to the measurement gas introduced from the buffer space 12 into the first internal space 20. When the measurement gas is introduced from the outside of the sensor element 101 to the first internal space 20, the measurement gas is suddenly taken into the sensor element 101 from the gas inlet 10 due to pressure fluctuations of the measurement gas in the external space (exhaust pressure pulsations if the measurement gas is automobile exhaust gas), but is not introduced directly into the first internal space 20, but is introduced into the first internal space 20 after the pressure fluctuations of the measurement gas are canceled through the first diffusion rate-controlling section 11, the buffer space 12, and the second diffusion rate-controlling section 13. As a result, the pressure fluctuations of the measurement gas introduced into the first internal space 20 are almost negligible. The first internal space 20 is provided as a space for adjusting the oxygen partial pressure in the measurement gas introduced through the second diffusion rate-controlling section 13. The oxygen partial pressure is adjusted by the operation of the main pump cell 21.
[0023] The main pump cell 21 is an electrochemical pump cell including an inner pump electrode 22 having a ceiling electrode portion 22a provided on almost the entire lower surface of the second solid electrolyte layer 6 facing the first internal space 20, an outer pump electrode 23 provided in a region corresponding to the ceiling electrode portion 22a on the upper surface of the second solid electrolyte layer 6 so as to be exposed to the external space, and the second solid electrolyte layer 6 sandwiched between these electrodes.
[0024] The inner pump electrode 22 is formed across the upper and lower solid electrolyte layers (the second solid electrolyte layer 6 and the first solid electrolyte layer 4) that define the first internal space 20, and the spacer layer 5 that provides the side walls. Specifically, a ceiling electrode portion 22a is formed on the lower surface of the second solid electrolyte layer 6 that provides the ceiling surface of the first internal space 20, and a bottom electrode portion 22b is formed on the upper surface of the first solid electrolyte layer 4 that provides the bottom surface. Side electrode portions (not shown) are formed on the side wall surfaces (inner surfaces) of the spacer layer 5 that constitute both side wall portions of the first internal space 20 so as to connect the ceiling electrode portion 22a and the bottom electrode portion 22b, and are arranged in a tunnel-shaped structure at the positions where the side electrode portions are arranged.
[0025] The inner pump electrode 22 and the outer pump electrode 23 are formed as porous cermet electrodes (for example, a cermet electrode of Pt containing 1% Au and ZrO2). The inner pump electrode 22, which comes into contact with the measurement gas, is formed using a material with a weakened ability to reduce the NOx component in the measurement gas.
[0026] In the main pump cell 21, by applying a desired voltage Vp0 between the inner pump electrode 22 and the outer pump electrode 23 and flowing a pump current Ip0 in a positive or negative direction between the inner pump electrode 22 and the outer pump electrode 23, it is possible to pump oxygen in the first internal space 20 out to the external space, or to pump oxygen from the external space into the first internal space 20.
[0027] In addition, in order to detect the oxygen concentration (oxygen partial pressure) in the atmosphere in the first internal space 20, an electrochemical sensor cell, i.e., an oxygen partial pressure detection sensor cell 80 for controlling the main pump, is configured by the inner pump electrode 22, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, and the reference electrode 42.
[0028] The oxygen concentration (oxygen partial pressure) in the first internal space 20 can be determined by measuring the electromotive force (voltage V0) in the main pump control oxygen partial pressure detection sensor cell 80. Furthermore, the pump current Ip0 is controlled by feedback controlling the voltage Vp0 of the variable power supply 24 so that the voltage V0 becomes a target value. This allows the oxygen concentration in the first internal space 20 to be maintained at a predetermined constant value.
[0029] The third diffusion rate-controlling section 30 is a section that applies a predetermined diffusion resistance to the measurement gas whose oxygen concentration (oxygen partial pressure) has been controlled by the operation of the main pump cell 21 in the first internal space 20, and guides the measurement gas to the second internal space 40.
[0030] The second internal space 40 is provided as a space for further adjusting the oxygen partial pressure by the auxiliary pump cell 50 for the measurement gas introduced through the third diffusion rate-controlling section 30 after the oxygen concentration (oxygen partial pressure) has been adjusted in advance in the first internal space 20. This makes it possible to keep the oxygen concentration in the second internal space 40 constant with high accuracy, thereby enabling the gas sensor 100 to measure the NOx concentration with high accuracy.
[0031] The auxiliary pump cell 50 is an auxiliary electrochemical pump cell composed of an auxiliary pump electrode 51 having a ceiling electrode portion 51a provided on almost the entire lower surface of the second solid electrolyte layer 6 facing the second internal space 40, an outer pump electrode 23 (not limited to the outer pump electrode 23, but any appropriate electrode on the outside of the sensor element 101 will suffice), and the second solid electrolyte layer 6.
[0032] The auxiliary pump electrode 51 is disposed in the second internal space 40 in a tunnel-shaped structure similar to that of the inner pump electrode 22 provided in the first internal space 20. That is, a ceiling electrode portion 51a is formed on the second solid electrolyte layer 6 providing the ceiling surface of the second internal space 40, a bottom electrode portion 51b is formed on the first solid electrolyte layer 4 providing the bottom surface of the second internal space 40, and side electrode portions (not shown) connecting the ceiling electrode portion 51a and the bottom electrode portion 51b are formed on both wall surfaces of the spacer layer 5 providing the side walls of the second internal space 40, respectively, forming a tunnel-shaped structure. Note that, like the inner pump electrode 22, the auxiliary pump electrode 51 is also formed using a material with a weakened ability to reduce NOx components in the measurement gas.
[0033] In the auxiliary pump cell 50, by applying a desired voltage Vp1 between the auxiliary pump electrode 51 and the outer pump electrode 23, it is possible to pump oxygen in the atmosphere within the second internal space 40 out to the external space or pump oxygen from the external space into the second internal space 40.
[0034] In addition, in order to control the oxygen partial pressure in the atmosphere within the second internal space 40, an electrochemical sensor cell, i.e., an oxygen partial pressure detection sensor cell 81 for controlling the auxiliary pump, is constituted by the auxiliary pump electrode 51, the reference electrode 42, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, and the third substrate layer 3.
[0035] The auxiliary pump cell 50 performs pumping using a variable power supply 52 whose voltage is controlled based on the electromotive force (voltage V1) detected by the auxiliary pump control oxygen partial pressure detection sensor cell 81. This allows the oxygen partial pressure in the atmosphere in the second internal space 40 to be controlled to a low partial pressure that does not substantially affect the measurement of NOx.
[0036] In addition, the pump current Ip1 is used to control the electromotive force of the main pump control oxygen partial pressure detection sensor cell 80. Specifically, the pump current Ip1 is input as a control signal to the main pump control oxygen partial pressure detection sensor cell 80, and the above-mentioned target value of the voltage V0 is controlled to always keep a constant gradient of the oxygen partial pressure in the measurement gas introduced from the third diffusion rate-controlling part 30 into the second internal space 40. When used as a NOx sensor, the oxygen concentration in the second internal space 40 is kept constant at about 0.001 ppm by the action of the main pump cell 21 and the auxiliary pump cell 50.
[0037] The fourth diffusion rate-controlling part 60 is a part that applies a predetermined diffusion resistance to the measurement gas whose oxygen concentration (oxygen partial pressure) has been controlled by the operation of the auxiliary pump cell 50 in the second internal space 40, and guides the measurement gas to the third internal space 61. The fourth diffusion rate-controlling part 60 serves to limit the amount of NOx flowing into the third internal space 61.
[0038] The third internal space 61 is provided as a space for carrying out a process for measuring the nitrogen oxide (NOx) concentration in the measurement gas, which has been introduced through the fourth diffusion-controlling part 60 after the oxygen concentration (oxygen partial pressure) has been adjusted in advance in the second internal space 40. The measurement of the NOx concentration is mainly carried out in the third internal space 61 by the operation of the measurement pump cell 41.
[0039] The measurement pump cell 41 measures the NOx concentration in the measurement gas in the third internal space 61. The measurement pump cell 41 is an electrochemical pump cell including a measurement electrode 44 provided on the upper surface of the first solid electrolyte layer 4 facing the third internal space 61, an outer pump electrode 23, the second solid electrolyte layer 6, a spacer layer 5, and the first solid electrolyte layer 4.
[0040] The measurement electrode 44 is a porous cermet electrode made of a material having a higher reduction capability for the NOx component in the measurement gas than the inner pump electrode 22. The measurement electrode 44 also functions as a NOx reduction catalyst that reduces NOx present in the atmosphere in the third internal space 61.
[0041] In the measurement pump cell 41, oxygen produced by decomposition of nitrogen oxides in the atmosphere surrounding the measurement electrode 44 is pumped out, and the amount of oxygen produced can be detected as a pump current Ip2.
[0042] In order to detect the oxygen partial pressure around the measurement electrode 44, an electrochemical sensor cell, i.e., an oxygen partial pressure detection sensor cell 82 for controlling the measurement pump, is configured by the first solid electrolyte layer 4, the third substrate layer 3, the measurement electrode 44, and the reference electrode 42. The variable power supply 46 is controlled based on the electromotive force (voltage V2) detected by the oxygen partial pressure detection sensor cell 82 for controlling the measurement pump.
[0043] The measurement gas introduced into the second internal space 40 reaches the measurement electrode 44 in the third internal space 61 through the fourth diffusion rate-controlling part 60 under the condition that the oxygen partial pressure is controlled. Nitrogen oxides in the measurement gas around the measurement electrode 44 are reduced (2NO→N2+O2) to generate oxygen. The generated oxygen is then pumped by the measurement pump cell 41, and the voltage Vp2 of the variable power supply 46 is controlled so that the voltage V2 detected by the measurement pump control oxygen partial pressure detection sensor cell 82 becomes constant (target value). The amount of oxygen generated around the measurement electrode 44 is proportional to the concentration of nitrogen oxides in the measurement gas, so that the nitrogen oxide concentration in the measurement gas is calculated using the pump current Ip2 in the measurement pump cell 41.
[0044] Furthermore, by combining the measurement electrode 44, the first solid electrolyte layer 4, the third substrate layer 3, and the reference electrode 42 to form an oxygen partial pressure detection means as an electrochemical sensor cell, it is possible to detect an electromotive force corresponding to the difference between the amount of oxygen generated by reduction of the NOx components in the atmosphere around the measurement electrode 44 and the amount of oxygen contained in the reference atmosphere, thereby making it possible to determine the concentration of the NOx components in the measured gas.
[0045] In addition, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, the outer pump electrode 23, and the reference electrode 42 constitute an electrochemical sensor cell 83, and the electromotive force (voltage Vref) obtained by this sensor cell 83 makes it possible to detect the oxygen partial pressure in the measured gas outside the sensor.
[0046] In the gas sensor 100 having such a configuration, the main pump cell 21 and the auxiliary pump cell 50 are operated to supply a measurement gas in which the oxygen partial pressure is always kept at a constant low value (a value that has substantially no effect on the measurement of NOx) to the measurement pump cell 41. Therefore, the NOx concentration in the measurement gas can be known based on the pump current Ip2 that flows when oxygen generated by the reduction of NOx is pumped out of the measurement pump cell 41, which is approximately proportional to the NOx concentration in the measurement gas.
[0047] Furthermore, the sensor element 101 includes a heater section 70 that adjusts the temperature by heating and keeping the sensor element 101 warm in order to increase the oxygen ion conductivity of the solid electrolyte. The heater section 70 includes a heater connector electrode 71, a heater 72, a through hole 73, a heater insulating layer 74, and a pressure release hole 75. The heater section 70 also includes a first substrate layer 1, a second substrate layer 2, and a third substrate layer 3 made of ceramics. The heater section 70 is configured as a ceramic heater including a heater 72, and the second substrate layer 2 and the third substrate layer 3 surrounding the heater 72. The heater 72 includes a heat generating section 76 and a lead section 85, as shown in FIG. 2.
[0048] The heater connector electrode 71 is an electrode formed in a manner to contact the lower surface of the first substrate layer 1. By connecting the heater connector electrode 71 to an external power source, it is possible to supply power to the heater section 70 from the outside.
[0049] The heat generating portion 76 of the heater 72 is an electrical resistor sandwiched between the second substrate layer 2 and the third substrate layer 3. The lead portion 85 of the heater 72 is connected to the heater connector electrode 71 via a through hole 73, and when power is supplied from the outside through the heater connector electrode 71, the heat generating portion 76 generates heat and heats and keeps warm the solid electrolyte that forms the sensor element 101.
[0050] In addition, the heat generating portion 76 of the heater 72 is embedded from the first internal space 20 to the third internal space 61, making it possible to adjust the temperature of the entire sensor element 101 to a temperature at which the solid electrolyte is activated.
[0051] The heater insulating layer 74 is an insulating layer made of an insulator such as alumina and formed on the upper and lower surfaces of the heater 72. The heater insulating layer 74 is formed for the purpose of obtaining electrical insulation between the second substrate layer 2 and the heater 72, and between the third substrate layer 3 and the heater 72.
[0052] The pressure relief hole 75 is a portion that penetrates the third substrate layer 3 and the atmosphere introduction layer 48 and is provided so as to communicate with the reference gas introduction space 43, and is formed for the purpose of mitigating the increase in internal pressure that accompanies an increase in temperature within the heater insulation layer 74.
[0053] The heating portion 76 and the lead portion 85 of the heater 72 will be described in detail. The heating portion 76 is a resistive heating element, and as shown in FIG. 2, has a strip-like shape with both ends connected to the lead portion 85. The heating portion 76 has a bent portion 77 and a straight portion 78. The bent portion 77 has a first bent portion 77a, a second bent portion 77b, and a third bent portion 77c. The straight portion 78 has a first outer straight portion 78a, a second outer straight portion 78b, a first inner straight portion 79a, and a second inner straight portion 79b. The multiple bent portions 77 and the multiple straight portions 78 are electrically connected in series. Specifically, starting from the first lead 85a, the first outer straight portion 78a, the first bent portion 77a, the first inner straight portion 79a, the second bent portion 77b, the second inner straight portion 79b, the third bent portion 77c, and the second outer straight portion 78b are connected in series with each other, and the second outer straight portion 78b is connected to the second lead 85b. The heat generating portion 76 has a symmetrical shape.
[0054] The straight portions 78 are arranged along the short-side direction (left-right direction) of the sensor element 101. Specifically, the first outer straight portion 78a, the first inner straight portion 79a, the second inner straight portion 79b, and the second outer straight portion 78b are arranged in this order from left to right of the sensor element 101. Therefore, the first inner straight portion 79a and the second inner straight portion 79b are arranged between the first outer straight portion 78a and the second outer straight portion 78b in the left-right direction. The first outer straight portion 78a, the second outer straight portion 78b, the first inner straight portion 79a, and the second inner straight portion 79b are all arranged so that their length directions are along the longitudinal direction. The rear end of the first outer straight portion 78a is connected to the first lead 85a, and the rear end of the second outer straight portion 78b is connected to the second lead 85b. The first inner straight portion 79a has a front portion 79a1, a rear portion 79a3 disposed rearward of the front portion 79a1, and a connecting portion 79a2 connecting the front portion 79a1 and the rear portion 79a3. The second inner straight portion 79b has a front portion 79b1, a rear portion 79b3 disposed rearward of the front portion 79b1, and a connecting portion 79b2 connecting the front portion 79b1 and the rear portion 79b3.
[0055] Regarding the straight portion 78, "disposed so that the length direction is along the longitudinal direction" includes a case where the length direction is parallel to the longitudinal direction (front-rear direction) of the sensor element 101 and a case where the length direction is inclined from the longitudinal direction (front-rear direction) of the sensor element 101. For example, in this embodiment, the length direction of the first outer straight portion 78a, the second outer straight portion 78b, the front portion 79a1, the rear portion 79a3, the front portion 79b1, and the rear portion 79b3 is parallel to the longitudinal direction of the sensor element 101. The length direction of the connection portion 79a2 and the connection portion 79b2 is inclined from the longitudinal direction of the sensor element 101.
[0056] Each of the plurality of bent portions 77 connects the straight portions 78 adjacent to each other in the left-right direction. Specifically, the first bent portion 77a connects the first outer straight portion 78a and the first inner straight portion 79a at one end side (here, the front side) in the longitudinal direction. The second bent portion 77b connects the first inner straight portion 79a and the second inner straight portion 79b at the other end side (here, the rear side) in the longitudinal direction. The third bent portion 77c connects the second inner straight portion 79b and the second outer straight portion 78b at one end side (here, the front side) in the longitudinal direction. The first to third bent portions 77a to 77c are all bent in a curved shape and have a semicircular arc shape. The first to third bent portions 77a to 77c may be bent in a broken line shape.
[0057] The positional relationship between the heat generating section 76 and the internal cavities (here, the first internal cavities 20, the second internal cavities 40, and the third internal cavities 61) of the measurement gas flow section is adjusted. This will be described. The first internal cavities 20 are an example of a main pump chamber, the second internal cavities 40 are an example of an auxiliary pump chamber, and the third internal cavities 61 are an example of a measurement chamber. In FIG. 2, the main pump chamber projection area Ap, which is an area obtained by projecting the first internal cavities 20 in the thickness direction (here, downward) toward the heat generating section 76, is shown by a dashed line frame. Similarly, the auxiliary pump chamber projection area Aq and the measurement chamber projection area Am, which are obtained by projecting the second internal cavities 40 and the third internal cavities 61 onto the heat generating section 76, are also shown by dashed line frames in FIG. 2. As shown in FIG. 2, in this embodiment, the main pump chamber projection area Ap, the auxiliary pump chamber projection area Aq, and the measurement chamber projection area Am are each a rectangular area. That is, in this embodiment, the first internal space 20, the second internal space 40, and the third internal space 61 each have a rectangular shape when viewed from above.
[0058] The first inner straight portion 79a and the second inner straight portion 79b of the heat generating portion 76 at least partially overlap with the main pump chamber projection region Ap. Specifically, a front portion 79a1 of the first inner straight portion 79a and a front portion 79b1 of the second inner straight portion 79b at least partially overlap with the main pump chamber projection region Ap. In other words, the first inner straight portion 79a and the second inner straight portion 79b (particularly the front portion 79a1 and the front portion 79b1) are present directly below the first internal space 20. Also, the first inner straight portion 79a and the second inner straight portion 79b of the heat generating portion 76 at least partially overlap with the auxiliary pump chamber projection region Aq. Specifically, a rear portion 79a3 of the first inner straight portion 79a and a rear portion 79b3 of the second inner straight portion 79b at least partially overlap with the auxiliary pump chamber projection region Aq. In other words, the first inner straight portion 79a and the second inner straight portion 79b (particularly the rear portion 79a3 and the rear portion 79b3) are present directly below the second internal space 40. In this embodiment, a part of the second bent portion 77b, specifically a part of the second bent portion 77b connected to the rear portion 79a3 and the rear portion 79b3, also overlaps with the auxiliary pump chamber projection area Aq. In addition, the heat generating portion 76 at least partially overlaps with the measurement chamber projection area Am. Specifically, the second bent portion 77b of the heat generating portion 76 at least partially overlaps with the measurement chamber projection area Am. In this embodiment, the connection portion 79a2 and the connection portion 79b2 are disposed between the main pump chamber projection area Ap and the auxiliary pump chamber projection area Aq in the front-rear direction, and do not overlap with the main pump chamber projection area Ap and the auxiliary pump chamber projection area Aq. Further, the first bent portion 77a, the third bent portion 77c, the first outer straight portion 78a, and the second outer straight portion 78b do not overlap with any of the main pump chamber projection area Ap, the auxiliary pump chamber projection area Aq, and the measurement chamber projection area Am, respectively. In this embodiment, the heat generating portion 76 is symmetrical, and the left and right central axes of the heat generating portion 76, the left and right central axes of the main pump chamber projection area Ap, the left and right central axes of the auxiliary pump chamber projection area Aq, and the left and right central axes of the measurement chamber projection area Am all coincide with each other.
[0059] The first inner straight portion 79a and the second inner straight portion 79b of the heat generating portion 76 have a mutual lateral (left-right) distance X1 in the portion overlapping with the main pump chamber projection region Ap that is equal to or greater than 1 / 3 of the lateral width Wp of the main pump chamber projection region Ap. That is, X1≧1 / 3×Wp is satisfied. In this embodiment, the portions of the heat generating portion 76 that overlap with the main pump chamber projection region Ap are the front portion 79a1 and the front portion 79b1, and therefore the left-right distance between the front portion 79a1 and the front portion 79b1 is the distance X1. Note that, in this embodiment, the length directions of the front portion 79a1 and the front portion 79b1 are parallel to each other, and therefore the left-right distance between the front portion 79a1 and the front portion 79b1 is a constant value (=distance X1). In cases where the left-right distance between the front portions 79a1 and 79b1 is not constant, for example when the front portions 79a1 and 79b1 are not parallel to each other, the average value of the short-side (left-right) distance between the first inner straight portion 79a and the second inner straight portion 79b at their portions that overlap with the main pump chamber projection area Ap is set to the distance X1.
[0060] The first inner straight portion 79a and the second inner straight portion 79b of the heat generating portion 76 have a mutual distance X2 in the short side direction (left-right direction) in the portion overlapping with the auxiliary pump chamber projection region Aq that is 0.4 times or more the width Wp in the short side direction of the main pump chamber projection region Ap. That is, X2≧0.4Wp is satisfied. In this embodiment, the rear portion 79a3 and the rear portion 79b3 of the heat generating portion 76 overlap with the auxiliary pump chamber projection region Aq, and therefore the left-right distance between the rear portion 79a3 and the rear portion 79b3 is the distance X2. Note that, in this embodiment, the rear portion 79a3 and the rear portion 79b3 are parallel to each other in the length direction, and therefore the left-right distance between the rear portion 79a3 and the rear portion 79b3 is a constant value (=distance X2). In cases where the rear portions 79a3 and 79b3 are not parallel to each other, or where the distance between them in the left-right direction is not constant, the average value of the distance between them in the short side direction (left-right direction) at the portions of the first inner straight portion 79a and the second inner straight portion 79b that overlap with the auxiliary pump chamber projection area Aq is set to the distance X2.
[0061] By satisfying the above conditions, i.e., "X1≧1 / 3×Wp" and "X2≧0.4Wp", stress occurring around the internal spaces (first internal space 20, second internal space 40, and third internal space 61) of the sensor element 101 when the heat generating portion 76 generates heat can be reduced. Moreover, the distance X1 is preferably 0.4 times or more the width Wp, and more preferably greater than 0.4 times. The distance X1 may be 2 / 3 times or more the width Wp. The distance X1 is preferably equal to or less than the width Wp, and may be less than the width Wp. The distance X2 may be 2 / 3 times or more the width Wp. Moreover, when the width in the left-right direction of the auxiliary pump chamber projection region Aq is the width Wq, the distance X2 is preferably equal to or less than the width Wq, and may be less than the width Wq. In this embodiment, as shown in FIG. 2, the distance X2 is greater than the distance X1.
[0062] In this embodiment, the heat generating portion 76 is symmetrical, and the left-right central axis of the heat generating portion 76 coincides with the left-right central axis of the main pump chamber projection area Ap. Therefore, the heat generating portion 76 does not exist in a region located in the left-right center of the main pump chamber projection area Ap and having a width equal to the distance X1. For example, when the above-mentioned X1>1 / 3×Wp is satisfied, the heat generating portion 76 does not exist in a region located in the left-right center of the main pump chamber projection area Ap and having a width of 1 / 3×Wp (i.e., the central region of the main pump chamber projection area Ap divided into three equal parts to the left and right). In other words, the heat generating portion 76 does not exist immediately below the region located in the left-right center of the main pump chamber (first internal space 20) and having a width of 1 / 3×Wp. Similarly, when the above-mentioned X1>0.4Wp is satisfied, the heat generating portion 76 does not exist in a region located in the left-right center of the main pump chamber projection area Ap and having a width of 0.4Wp.
[0063] Furthermore, since the heat generating portion 76 is symmetrical and the left-right central axis of the heat generating portion 76 coincides with the left-right central axis of the main pump chamber projection area Ap, if the distance X1 is equal to or less than the width Wp, the first inner straight portion 79a and the second inner straight portion 79b (here, particularly the front portion 79a1 and the front portion 79b1) will each overlap at least partially with the main pump chamber projection area Ap.
[0064] In this embodiment, the heat generating portion 76 is symmetrical, and the left-right central axis of the heat generating portion 76 coincides with the left-right central axis of the auxiliary pump chamber projection area Aq. Therefore, the heat generating portion 76 does not exist in an area that is located in the left-right center of the auxiliary pump chamber projection area Aq and has a width equal to the distance X2. In other words, the heat generating portion 76 does not exist directly below the area that is in the left-right center of the auxiliary pump chamber (second internal space 40) and has a width of X2.
[0065] Furthermore, since the heat generating portion 76 is symmetrical and the left-right central axis of the heat generating portion 76 coincides with the left-right central axis of the auxiliary pump chamber projection area Aq, if the distance X2 is equal to or less than the width Wq, the first inner straight portion 79a and the second inner straight portion 79b (particularly the rear portion 79a3 and the rear portion 79b3 in this case) will each overlap at least partially with the auxiliary pump chamber projection area Aq.
[0066] In this embodiment, the heating portion 76 is a cermet containing a precious metal and a ceramic (for example, a cermet of platinum (Pt) and alumina (Al2O3)). The heating portion 76 is not limited to a cermet, and may be any material that contains a conductive material such as a precious metal. The precious metal used in the heating portion 76 may be at least one of platinum, rhodium (Rh), gold (Au), and palladium (Pd), or an alloy thereof.
[0067] Here, the resistance value per unit length of the pump chamber overlapping portion, which is the portion of the heat generating portion 76 that overlaps with the main pump chamber projection area Ap and the auxiliary pump chamber projection area Aq, is defined as unit resistance value R1 [μΩ / mm]. Also, the resistance value per unit length of the measurement chamber overlapping portion, which is the portion of the heat generating portion 76 that overlaps with the measurement chamber projection area Am, is defined as unit resistance value R3 [μΩ / mm]. In this case, the heat generating portion 76 has a unit resistance value ratio R3 / R1 less than 1 at least at any temperature in the temperature range of 700°C to 900°C, which is a temperature range in which the heat generating portion 76 may be heated during use. In other words, the unit resistance value R3 is lower than the unit resistance value R1 at least at any temperature in the temperature range of 700°C to 900°C. In this embodiment, the pump chamber overlapping portion is composed of a portion of the front portion 79a1 and the front portion 79b1 that overlaps with the main pump chamber projection region Ap, a portion of the rear portion 79a3 and the rear portion 79b3 that overlaps with the auxiliary pump chamber projection region Aq, and a portion of the second bend portion 77b that overlaps with the auxiliary pump chamber projection region Aq. In this embodiment, the measurement chamber overlapping portion is a portion of the second bend portion 77b that overlaps with the measurement chamber projection region Am. The length direction of the heat generating portion 76 is the axial direction of the heat generating portion 76, in other words, the direction in which the current flows. The unit resistance value R1 is the average value of the resistance value per unit length of the pump chamber overlapping portion. Similarly, the unit resistance value R3 is the average value of the resistance value per unit length of the measurement chamber overlapping portion. Therefore, even if there is a portion of the measurement chamber overlapping portion that has a higher resistance value per unit length than the pump chamber overlapping portion, it is sufficient that the measurement chamber overlapping portion has a lower resistance value per unit length overall. However, it is preferable that the resistance per unit length at any position in the overlapping portion of the measurement chambers is lower than the unit resistance R1.
[0068] If the unit resistance value R3 is too large, the difference between the temperature around the first internal space 20 and the second internal space 40 and the temperature around the third internal space 61 becomes too small, which may result in a decrease in the detection accuracy of the NOx concentration. By making the unit resistance value ratio R3 / R1 less than 1, such a decrease in detection accuracy can be suppressed. The unit resistance value ratio R3 / R1 at least at any temperature in the above temperature range is preferably 0.8 or less, more preferably 0.7 or less, and even more preferably 0.65 or less. The unit resistance value ratio R3 / R1 at least at any temperature in the above temperature range may be 0.5 or more.
[0069] In this embodiment, the first inner straight portion 79a, the second inner straight portion 79b, and the second bent portion 77b are made of the same material (the above-mentioned platinum-containing cermet), and the cross-sectional area S1 [mm 2 ] is the cross-sectional area S3 [mm 2 ]. That is, the heat generating portion 76 has a cross-sectional area ratio S1 / S3 less than 1. In this way, the unit resistance value ratio R3 / R1 is less than 1 in any temperature range from 700°C to 900°C. The cross-sectional area ratio S1 / S3 is preferably 0.8 or less, more preferably 0.7 or less, and even more preferably 0.65 or less. The cross-sectional area ratio S1 / S3 may be 0.5 or more. The cross-sectional area ratio S1 / S3 may be adjusted, for example, by making the width W1 of the pump chamber overlapping portion smaller than the width W3 of the measurement chamber overlapping portion, or by making the thickness D1 of the pump chamber overlapping portion smaller than the thickness D3 of the measurement chamber overlapping portion. The cross-sectional areas S1, S3, widths W1, W3, and thicknesses D1, D3 are all set to the average values of the pump chamber overlapping portion and the measurement chamber overlapping portion, as are the unit resistance values R1, R3.
[0070] In this embodiment, the first inner straight portion 79a, the second inner straight portion 79b, and the second bent portion 77b have the same thickness in all parts. The first inner straight portion 79a and the second inner straight portion 79b have the same width in all parts. In addition, the second bent portion 77b has a width that increases as it moves away from the first inner straight portion 79a and the second inner straight portion 79b at the connecting portion with the first inner straight portion 79a and the second inner straight portion 79b, and has a constant width in the portion other than the connecting portion (including the portion overlapping with the measurement chamber projection area Am). Therefore, the width W1 in this embodiment is slightly larger than the width of the first inner straight portion 79a and the second inner straight portion 79b by the amount that a part of the second bent portion 77b is included in the pump chamber overlapping portion. In addition, the width W3 is the same as the width of the portion of the second bent portion 77b other than the connecting portion with the first inner straight portion 79a and the second inner straight portion 79b. Since the width W1 is smaller than the width W3, the cross-sectional area ratio S1 / S3 is less than 1. The ratio W1 / W3 of the width W1 to the width W3 is preferably 0.8 or less, more preferably 0.7 or less, and even more preferably 0.65 or less. The ratio W1 / W3 may be 0.5 or more. The widths W1 and W3 may be 0.05 mm or more and 1.5 mm or less. The thicknesses D1 and D3 may be 0.003 mm or more and 0.1 mm or less. The width W1 may be 0.3 mm or more and 0.4 mm or less. The width W3 may be 0.5 mm or more and 0.6 mm or less.
[0071] The distance X1 may be 0.67 mm or more, 0.8 mm or more, or 0.86 mm or more. The distance X1 may be 2 mm or less, less than 2 mm, 1.67 mm or less, or 1.34 mm or less. The distance X2 may be 0.8 mm or more, or 0.86 mm or more. The distance X2 may be 2 mm or less, less than 2 mm, or 1.34 mm or less. The width Wp (= the width of the first internal space 20) of the main pump chamber projection region Ap is, for example, 1.5 mm or more and 3 mm or less. The width Wq (= the width of the second internal space 40) of the auxiliary pump chamber projection region Aq is, for example, 1.2 mm or more and 2.4 mm or less. The width Wm (= the width of the third internal space 61) of the measurement chamber projection region Am is, for example, 0.9 mm or more and 1.8 mm or less. The length from the front end of the sensor element 101 to the rear end of the third internal space 61, that is, the length of the measurement gas flow portion, is, for example, 7.5 mm to 9 mm. In this embodiment, Wp>Wq>Wm is satisfied.
[0072] The lead portion 85 has a first lead 85a disposed on the left rear side of the heat generating portion 76 and a second lead 85b disposed on the right rear side. The first and second leads 85a and 85b are leads for passing electricity to the heat generating portion 76 and are connected to the heater connector electrode 71. The first lead 85a is a positive electrode lead and the second lead 85b is a negative electrode lead. When a voltage is applied between the first and second leads 85a and 85b, a current flows through the heat generating portion 76 and the heat generating portion 76 generates heat. The lead portion 85 is a conductor and has a lower resistance per unit length than the heat generating portion 76. Therefore, unlike the heat generating portion 76, the lead portion 85 hardly generates heat when electricity is applied. For example, the lead portion 85 has a lower resistance per unit length because it is made of a material with a lower volume resistivity than the heat generating portion 76 or has a larger cross-sectional area. In this embodiment, the lead portion 85 has a higher proportion of precious metal than the heat generating portion 76, resulting in a lower volume resistivity, and is wider than the heat generating portion 76, resulting in a larger cross-sectional area.
[0073] A method for manufacturing the gas sensor 100 thus constructed is described below. First, six unfired ceramic green sheets containing an oxygen ion conductive solid electrolyte such as zirconia as a ceramic component are prepared. A plurality of sheet holes and necessary through holes used for positioning during printing and lamination are formed in advance in the green sheets. A space to be a measurement gas flow section is also provided in advance in the green sheets to be the spacer layer 5 by punching or the like. Then, a pattern printing process and drying process are performed to form various patterns on each ceramic green sheet corresponding to each of the first substrate layer 1, the second substrate layer 2, the third substrate layer 3, the first solid electrolyte layer 4, the spacer layer 5, and the second solid electrolyte layer 6. Specifically, the patterns to be formed are, for example, the patterns of the above-mentioned electrodes, the lead wires connected to each electrode, the air introduction layer 48, the heater 72, and the like. The pattern printing is performed by applying a pattern forming paste prepared according to the characteristics required for each formation target onto the green sheets using a known screen printing technique. The paste for forming the pattern that becomes the heater 72 is made by mixing the raw material (for example, precious metal and ceramic particles) made of the material of the heater 72 described above, an organic binder, an organic solvent, and the like.
[0074] At this time, the pattern that becomes the heater 72 is formed so that the unit resistance value ratio R3 / R1 is less than 1, for example, so that the cross-sectional area ratio S1 / S3 is less than 1. For example, to make the width W1<width W3, a mask having a shape that can form such a pattern is used. Also, to make the thickness D1<thickness D3, for example, the viscosity of the paste that forms the pattern of the portion that becomes the measurement chamber overlapping portion (e.g., the second bent portion 77b) is made higher than the pattern of the portion that becomes the pump chamber overlapping portion (e.g., the first inner straight portion 79a and the second inner straight portion 79b), or the number of printing operations when forming the pattern of the portion that becomes the measurement chamber overlapping portion is increased.
[0075] After forming various patterns in this way, the green sheets are dried. The drying process is also performed using a known drying means. After the pattern printing and drying is completed, a printing and drying process of an adhesive paste for laminating and bonding the green sheets corresponding to each layer is performed. Then, the green sheets on which the adhesive paste has been formed are laminated in a predetermined order while being positioned by the sheet holes, and are pressed by applying predetermined temperature and pressure conditions to form one laminate. The laminate thus obtained contains a plurality of sensor elements 101. The laminate is cut to the size of the sensor element 101. The cut laminate is then fired at a predetermined firing temperature to obtain the sensor element 101.
[0076] Once the sensor element 101 is obtained in this manner, a sensor assembly incorporating the sensor element 101 is manufactured, and a protective cover or the like is attached to obtain the gas sensor 100.
[0077] In the gas sensor 100 thus constructed, when in use, the heater 72 is connected to a power source (e.g., an alternator of an automobile) via the heater connector electrode 71, and a DC voltage (e.g., 12 to 14 V) is applied between the first lead 85a and the second lead 85b. Then, the applied voltage causes a current to flow through the heating portion 76, which generates heat. As a result, the entire sensor element 101 is adjusted to a temperature (e.g., 700°C to 900°C) at which the solid electrolyte (each of the layers 1 to 6) is activated. In this state, when the measurement gas is introduced from the gas inlet 10 into the measurement gas flow portion, the measurement gas passes through the first diffusion rate-controlling portion 11, the buffer space 12, and the second diffusion rate-controlling portion 13, and reaches the first internal space 20. Next, the oxygen concentration of the measurement gas is adjusted by the main pump cell 21 and the auxiliary pump cell 50 in the first internal space 20 and the second internal space 40, and the adjusted measurement gas reaches the third internal space 61. The NOx concentration in the measurement gas is detected based on the pump current Ip2 when the measurement pump cell 41 pumps out oxygen from the third internal space 61.
[0078] At this time, the heat generating portion 76 becomes hot, and stress may be generated around the internal cavities (the first internal cavities 20, the second internal cavities 40, and the third internal cavities 61) of the sensor element 101. This is considered to be due to the temperature difference between the lower side of the internal cavities and the upper side of the internal cavities of the sensor element 101. However, in the sensor element 101 of this embodiment, by satisfying the above-mentioned "X1 ≧ 1 / 3 × Wp" and "X2 ≧ 0.4 Wp", the stress generated around the internal cavities of the sensor element 101 when the heat generating portion 76 generates heat can be reduced. This is considered to be because the distances X1 and X2 satisfy the above-mentioned conditions, and therefore overheating of the lower side of the internal cavities near the center on the left and right can be suppressed, and the temperature difference between the lower side of the internal cavities and the upper side of the internal cavities can be reduced. In addition, if the distance X1 is greater than 0.4 times the width Wp, the effect of reducing the above-mentioned stress is enhanced.
[0079] Furthermore, by satisfying "X1≧1 / 3×Wp" and "X2≧0.4Wp", it is possible to reduce stress generated in the outer periphery of the sensor element 101 (particularly, the underside, which is the outer periphery of the sensor element 101 closest to the heater 72). This is presumably because, by making the distances X1 and X2 satisfy the above conditions, it is possible to prevent the left and right centers of the underside of the sensor element 101 from overheating, thereby reducing the temperature difference between the left and right centers of the underside and the rest.
[0080] In the present embodiment, the distance X1 is equal to or less than the width Wp, and the first inner straight portion 79a and the second inner straight portion 79b (particularly the front portion 79a1 and the front portion 79b1 here) at least partially overlap with the main pump chamber projection area Ap. Therefore, the heat generating portion 76 can sufficiently heat the solid electrolyte around the main pump chamber (the first internal space 20 here), and the main pump cell 21 can function sufficiently. Similarly, the distance X2 is equal to or less than the width Wq, and the first inner straight portion 79a and the second inner straight portion 79b (particularly the rear portion 79a3 and the rear portion 79b3 here) at least partially overlap with the auxiliary pump chamber projection area Aq. Therefore, the heat generating portion 76 can sufficiently heat the solid electrolyte around the auxiliary pump chamber (the second internal space 40 here), and the auxiliary pump cell 50 can function sufficiently. If the functions of the main pump cell 21 and the auxiliary pump cell 50 are insufficient, the oxygen concentration in the measured gas may not be sufficiently adjusted, and the detection accuracy of the NOx concentration may decrease. However, in this embodiment, the distance X1 is equal to or less than the width Wp and the distance X2 is equal to or less than the width Wq, thereby suppressing the decrease in the detection accuracy of the NOx concentration.
[0081] In addition, in this embodiment, since the heat generating portion 76 (here, the second bent portion 77b) at least partially overlaps with the measurement chamber projection area Am, the solid electrolyte around the measurement chamber (here, the third internal space 61) can be sufficiently heated, and the measurement pump cell 41 can function sufficiently. This also makes it possible to suppress a decrease in the detection accuracy of the NOx concentration.
[0082] In addition, since the unit resistance ratio R3 / R1 is less than 1 at least at any temperature in the temperature range of 700°C to 900°C, the deterioration of the detection accuracy of the NOx concentration can be suppressed. This will be explained in detail. First, assuming that the temperatures around the first internal space 20, the second internal space 40, and the third internal space 61 are temperatures Tp, Tq, and Tm [°C], respectively, when the heat generating part 76 generates heat, it is preferable that (temperature Tp and temperature Tq)>temperature Tm, and it is more preferable that temperature Tp>temperature Tq>temperature Tm. This is for the following reason. The oxygen concentration is higher around the inner pump electrode 22, i.e., the first internal space 20, than around the measurement electrode 44 because the measurement target gas before the oxygen concentration adjustment by the main pump cell 21 flows in from the gas inlet 10 side. In addition, the periphery of the auxiliary pump electrode 51, i.e., the second internal space 40, has a higher oxygen concentration than the periphery of the measurement electrode 44, because the measurement gas before the oxygen concentration adjustment by the auxiliary pump cell 50 flows in from the first internal space 20 side. Therefore, it is preferable to make the temperature Tp around the first internal space 20 and the temperature Tq around the second internal space 40 higher than the temperature Tm, so that the main pump cell 21 and the auxiliary pump cell 50 can pump out a large amount of oxygen, and to further activate the inner pump electrode 22, the auxiliary pump electrode 51, and the solid electrolyte layer around them. On the other hand, the periphery of the measurement electrode 44, i.e., the third internal space 61, has a lower oxygen concentration than the first internal space 20 and the second internal space 40. Therefore, for example, hydrogen and carbon monoxide may be generated by reduction of water and carbon dioxide in the measurement gas, and these may chemically react with oxygen in NOx, resulting in a decrease in measurement accuracy. The higher the temperature, the more likely such reduction of components other than the specific gas (NOx) occurs. Therefore, it is preferable that the temperature Tm is not too high. From the above, it is preferable that (temperature Tp and temperature Tq)>temperature Tm. Furthermore, since the first internal space 20 is located upstream of the measurement gas flow section relative to the second internal space 40 and the oxygen concentration in the first internal space 20 is higher than that in the second internal space 40, it is preferable to make the temperature Tp around the first internal space 20 higher than the temperature Tq around the second internal space 40 to further activate the inner pump electrode 22 and the solid electrolyte layer around it. Therefore, it is more preferable that temperature Tp>temperature Tq>temperature Tm.If the unit resistance value R3 is too large, the temperature Tm becomes too high and the relationship (temperature Tp and temperature Tq) > temperature Tm is not satisfied, and the measurement accuracy of the NOx concentration may decrease. Since the unit resistance value ratio R3 / R1 is less than 1, the unit resistance value R3 is not too large, and such a decrease in detection accuracy can be suppressed. Furthermore, if the temperature Tm is high, the temperature Tq around the second internal space 40 close to the third internal space 61 is also likely to become high, so that the temperature Tp < temperature Tq > temperature Tm, and the relationship of temperature Tp > temperature Tq > temperature Tm is not satisfied, and the pumping capacity of the main pump cell 21 may be insufficient. On the other hand, if the unit resistance value ratio R3 / R1 is less than 1, the pumping capacity of the main pump cell 21 is likely to be sufficiently high.
[0083] Here, the correspondence between the components of this embodiment and the components of the present invention will be clarified. Each layer 1 to 6 in this embodiment corresponds to the element body of the present invention, the first internal space 20 corresponds to the main pump chamber, the main pump cell 21 corresponds to the main pump cell, the second internal space 40 corresponds to the auxiliary pump chamber, the auxiliary pump cell 50 corresponds to the auxiliary pump cell, the third internal space 61 corresponds to the measurement chamber, the measurement pump cell 41 corresponds to the measurement pump cell, the heat generating portion 76 corresponds to the heat generating element, the first outer straight portion 78a corresponds to the first outer straight portion, the second outer straight portion 78b corresponds to the second outer straight portion, the first inner straight portion 79a corresponds to the first inner straight portion, the second inner straight portion 79b corresponds to the second inner straight portion, the first to third bent portions 77a to 77c correspond to the first to third bent portions, the main pump chamber projected area Ap corresponds to the main pump chamber projected area, and the auxiliary pump chamber projected area Aq corresponds to the auxiliary pump chamber projected area.
[0084] According to the gas sensor 100 of the present embodiment described above in detail, the distance X1 is ⅓ or more of the width Wp, and the distance X2 is 0.4 times or more of the width Wp, so that the stress generated around the internal space (the main pump chamber, the auxiliary pump chamber, and the measurement chamber) when the heating element generates heat can be reduced. Furthermore, the distance X1 is more than 0.4 times the width Wp, so that the effect of reducing the above-mentioned stress is enhanced. Furthermore, the unit resistance value ratio R3 / R1 is less than 1 at least at any temperature in the temperature range of 700°C to 900°C, so that the deterioration of the detection accuracy of the NOx concentration can be suppressed.
[0085] It goes without saying that the present invention is not limited to the above-described embodiment, and can be embodied in various forms within the technical scope of the present invention.
[0086] For example, in the above-described embodiment, the distance X2 is greater than the distance X1, but this is not limited thereto. For example, the distance X1 and the distance X2 may be the same size as shown in FIG. 3. In this case, too, by satisfying "X1≧1 / 3×Wp" and "X2≧0.4Wp", the effect of reducing the stress generated around the internal space of the sensor element 101 when the heat generating portion 76 generates heat can be obtained. In the case of FIG. 3, since X1=X2, "X1≧0.4Wp" is also satisfied. In addition, in the example of FIG. 3, the front portion 79a1, the connection portion 79a2, and the rear portion 79a3 of the first inner straight portion 79a are arranged in a straight line, so that the front portion 79a1, the connection portion 79a2, and the rear portion 79a3 have shapes that cannot be distinguished from one another. The same is true for the front portion 79b1, the connection portion 79b2, and the rear portion 79b3 of the second inner straight portion 79b.
[0087] Alternatively, distance X1 may be greater than distance X2 as shown in Fig. 4. In this case as well, by satisfying "X1 ≥ 1 / 3 × Wp" and "X2 ≥ 0.4 Wp", it is possible to obtain the effect of reducing the stress generated around the internal space of sensor element 101 when heat is generated by heat generating portion 76. In the case of Fig. 4, since X1 > X2, "X1 > 0.4 Wp" is also satisfied.
[0088] In the above-described embodiment, the cross-sectional area ratio S1 / S3 is set to a value less than 1, thereby making the unit resistance value ratio R3 / R1 less than 1, but this is not limited thereto. For example, the volume resistivity ratio ρ3 / ρ1, which is the ratio of the volume resistivity ρ1 [μΩ·cm] of the pump chamber overlapping portion to the volume resistivity ρ3 [μΩ·cm] of the measurement chamber overlapping portion, may be less than 1 at least at any temperature in the above-described temperature range. Even in this case, the unit resistance value ratio R3 / R1 can be set to a value less than 1 at least at any temperature in the above-described temperature range, and the deterioration of the detection accuracy of the NOx concentration can be suppressed. At least at any temperature in the above-described temperature range, the volume resistivity ratio ρ3 / ρ1 is preferably 0.8 or less, more preferably 0.7 or less, and even more preferably 0.65 or less. The volume resistivity ratio ρ3 / ρ1 may be 0.5 or more. For example, the volume resistivity ρ3 can be made lower than the volume resistivity ρ1 by increasing the ratio of the precious metal (conductor) contained in the measurement chamber overlapping portion of the heat generating portion 76 compared to the pump chamber overlapping portion. The volume resistivities ρ1 and ρ3 are the average values of the pump chamber overlapping portion and the measurement chamber overlapping portion, similar to the unit resistances R1 and R3.
[0089] In the above-described embodiment, the unit resistance value R3 / R1 is set to a value less than 1, but is not limited to this. For example, in Fig. 2, the width of the second bent portion 77b may be set to the same as the widths of the first inner straight portion 79a and the second inner straight portion 79b, and the unit resistance value R3 / R1 may be set to a value of 1. In this case as well, as long as "X1 ≥ 1 / 3 × Wp" and "X2 ≥ 0.4 Wp" are satisfied, the effect of reducing the stress generated around the internal space of the sensor element 101 when the heat generating portion 76 generates heat can be obtained.
[0090] In the above-described embodiment, the heat generating portion 76 is symmetrical, and the left and right central axes of the heat generating portion 76, the left and right central axes of the main pump chamber projection region Ap, the left and right central axes of the auxiliary pump chamber projection region Aq, and the left and right central axes of the measurement chamber projection region Am all coincide with each other, but this is not particularly limited. For example, the heat generating portion 76 may be asymmetrical, or any of the above central axes may be shifted from the other central axes. In this case, it is sufficient that at least a portion of each of the first inner straight portion 79a and the second inner straight portion 79b overlaps with the main pump chamber projection region Ap, and at least a portion of each of the first inner straight portion 79a and the second inner straight portion 79b overlaps with the auxiliary pump chamber projection region Aq, and "X1 ≧ 1 / 3 × Wp" and "X2 ≧ 0.4 Wp" are satisfied.
[0091] In the above-described embodiment, the shape of the main pump chamber projection region Ap, i.e., the shape of the first internal space 20 in top view, is rectangular, and the width in the short-side direction of the main pump chamber projection region Ap is a constant value (=width Wp) as shown in Fig. 2, but this is not limited to this. For example, the width in the short-side direction of the main pump chamber projection region Ap may not be constant, such as when there are parts where the width in the short-side direction of the main pump chamber projection region Ap is large and parts where it is small. In such a case, the maximum value of the width in the short-side direction of the main pump chamber projection region Ap is set to the width Wp. The same is true for the width Wq of the auxiliary pump chamber projection region Aq and the width Wm of the measurement chamber projection region Am. EXAMPLES
[0092] Specific examples of sensor elements produced will be described below as examples. Experimental Examples 3 to 6, 8, 9, and 10 correspond to examples of the present invention, and Experimental Examples 1, 2, 7, and 11 correspond to comparative examples. Note that the present invention is not limited to the following examples.
[0093] [Experimental Example 1] A sensor element similar to the sensor element 101 shown in Figs. 1 and 2 was used as Experimental Example 1, except that "X1 ≥ 1 / 3 × Wp" was not satisfied. The size of the sensor element of Experimental Example 1 was 67.5 mm in length in the front-rear direction, 4.25 mm in width in the left-right direction, and 1.45 mm in thickness in the up-down direction. The widths of the first outer straight portion 78a and the second outer straight portion 78b were 0.28 mm. The widths of the first inner straight portion 79a and the second inner straight portion 79b were 0.33 mm. The width of the second bend portion 77b other than the connection portion with the first inner straight portion 79a and the second inner straight portion 79b was 0.53 mm. The width Wp of the main pump chamber projection area Ap was 2 mm. The width Wq of the auxiliary pump chamber projection area Aq was 1.6 mm. The width Wm of the measurement chamber projection area Am was 1.2 mm. The length of the measurement gas flow portion was 8.3 mm. The distance X1 was set to 0.26 mm (=0.13 Wp), and the distance X2 was set to 0.86 mm (=0.43 Wp). Therefore, Experimental Example 1 satisfies "X2≧0.4 Wp", but does not satisfy "X1≧1 / 3×Wp".
[0094] [Experimental Examples 2 and 3] The same sensor element as in Experimental Example 1 was used as Experimental Example 2, except that the distance X1 was set to 0.46 mm (=0.23 Wp). The same sensor element as in Experimental Example 1 was used as Experimental Example 3, except that the distance X1 was set to 0.67 mm (=1 / 3×Wp).
[0095] [Experimental Example 4] A sensor element having a heater 72 pattern as shown in Fig. 3 was used as Experimental Example 4. In Experimental Example 4, the distance X1 and the distance X2 were both set to 0.86 mm (=0.43 Wp). The other dimensions were the same as those of Experimental Example 1.
[0096] [Experimental Examples 5 and 6] The sensor elements having the heater 72 pattern shown in FIG. 4 were used as Experimental Examples 5 and 6. In Experimental Example 5, the distance X1 was set to 1.34 mm (= 2 / 3 × Wp) and the distance X2 was set to 0.86 mm (= 0.43 Wp). In Experimental Example 6, the distance X1 was set to 1.67 mm (= 0.84 Wp) and the distance X2 was set to 0.86 mm (= 0.43 Wp). Other dimensions of Experimental Examples 5 and 6 were the same as those of Experimental Example 1.
[0097] [Experimental Examples 7-9] Experimental Examples 7 to 9 were sensor elements in which the heater 72 had a pattern as shown in FIG. 3. In Experimental Example 7, the distances X1 and X2 were both 0.67 mm (= 1 / 3 × Wp). In Experimental Example 8, the distances X1 and X2 were both 1.34 mm (= 2 / 3 × Wp). In Experimental Example 9, the distances X1 and X2 were both 0.8 mm (= 0.4 Wp). Other dimensions in Experimental Examples 7 to 9 were the same as in Experimental Example 1.
[0098] [Stress Evaluation] For each of the sensor elements of Experimental Examples 1 to 9, the stress in the internal space and the stress in the outer periphery of the sensor element were examined when the heating portion 76 was heated to 800°C. The stress in the internal space was defined as the maximum value of the stress generated around the first internal space 20, the second internal space 40, and the third internal space 61 of the sensor element, and the sensor element was evaluated in four stages, "Excellent (A)", "Good (B)", "Fair (C)", and "Fail (F)", depending on the magnitude of this maximum value. The stress in the outer periphery was defined as the maximum value of the stress generated on the lower surface of the sensor element, and the sensor element was evaluated in four stages, "Excellent (A)", "Good (B)", "Fail (C)", and "Fail (F)", depending on the magnitude of this maximum value. In each evaluation, "Excellent (A)" had the smallest maximum value of stress, and "Fail (F)" had the largest maximum value of stress.
[0099] The results of the stress evaluation of the distances X1 and X2, the internal void, and the stress evaluation of the outer periphery for each of the experimental examples 1 to 9 are shown in Table 1 and Figures 5 and 6. Figure 5 shows the results of the stress evaluation of the internal void, and Figure 6 shows the results of the stress evaluation of the outer periphery. The numbers 1 to 9 in Figures 5 and 6 represent the numbers of each experimental example. The results of the stress evaluation are shown as follows: "Excellent (A)" is shown with a circle, "Good (B)" with a white square, "Fair (C)" with a hatched square, and "Fail (F)" with a black square.
[0100] [Table 1]
[0101] As can be seen from Table 1 and FIG. 5, in Experimental Examples 1 and 2, which do not satisfy the former of "X1 ≧ 1 / 3 × Wp" and "X2 ≧ 0.4Wp", and Experimental Example 7, which does not satisfy the latter, the stress evaluation of the internal void was "Fail (F)". In contrast, in Experimental Examples 3 to 6, 8, and 9, which satisfy both "X1 ≧ 1 / 3 × Wp" and "X2 ≧ 0.4Wp", the stress evaluation of the internal void was "Fair (C)" or higher. From these results, it was confirmed that the stress of the internal void can be reduced by satisfying both "X1 ≧ 1 / 3 × Wp" and "X2 ≧ 0.4Wp". Furthermore, in Experimental Examples 4 to 6 and 8, which further satisfy "X1>0.4Wp", the stress evaluation of the internal void was "Good (B)" or higher. Also, as can be seen from FIG. 5, it was confirmed that the greater the distances X1 and X2, that is, the closer the experimental example is plotted to the upper right of FIG. 5, the higher the stress evaluation of the internal void tends to be.
[0102] The stress evaluation of the outer periphery showed a tendency similar to that of the internal space. Specifically, as can be seen from Table 1 and FIG. 6, in Experimental Examples 1 and 2, which do not satisfy the former of "X1 ≧ 1 / 3 × Wp" and "X2 ≧ 0.4Wp", and Experimental Example 7, which does not satisfy the latter, the stress evaluation of the outer periphery was "Fail (F)". In contrast, in Experimental Examples 3 to 6, 8, and 9, which satisfy both "X1 ≧ 1 / 3 × Wp" and "X2 ≧ 0.4Wp", the stress evaluation of the outer periphery was "Fair (C)" or higher. From these results, it was confirmed that the stress of the outer periphery can be reduced by satisfying both "X1 ≧ 1 / 3 × Wp" and "X2 ≧ 0.4Wp". In addition, as can be seen from FIG. 6, it was confirmed that the larger the distances X1 and X2 are, that is, the higher the stress evaluation of the outer periphery is, the more the experimental examples are plotted in the upper right of FIG. 6.
[0103] [Experimental Example 10] A sensor element having a heater 72 pattern shaped as shown in Fig. 3 was used as Experimental Example 10. In Experimental Example 10, similar to Experimental Example 4, the distances X1 and X2 were both set to 0.86 mm (=0.43 Wp). The other dimensions were the same as in Experimental Example 1. Therefore, Experimental Example 10 satisfies both "X1 ≥ 1 / 3 × Wp" and "X2 ≥ 0.4 Wp".
[0104] [Experimental Example 11] A sensor element having a heater 72 pattern as shown in FIG. 7 was used as Experimental Example 11. In Experimental Example 11, as shown in FIG. 7, the first inner straight portion 79a and the second inner straight portion 79b have a shape in which the widths are partially large, and the widths of the portions overlapping with the auxiliary pump chamber projection area Aq are the largest. The front portion 79a1 of the first inner straight portion 79a has a portion whose length direction is inclined from the longitudinal direction (front-rear direction) of the sensor element and a portion parallel to the longitudinal direction (front-rear direction). The front portion 79b1 of the second inner straight portion 79b is similar. The portion of the front portion 79a1 inclined from the longitudinal direction and the portion of the front portion 79b1 inclined from the longitudinal direction are arranged such that the left-right distance between them increases as they approach the front end of the sensor element. The left-right distance between the front portion 79a1 and the front portion 79b1 is not constant, and the left-right distance between the portion of the front portion 79a1 parallel to the front-back direction and the portion of the front portion 79b1 parallel to the front-back direction is the minimum left-right distance X1min between the front portion 79a1 and the front portion 79b1. The minimum distance X1min was set to 0.47 mm. The distance X1 is the average value of the short-side (left-right) distance between the first inner straight portion 79a and the second inner straight portion 79b in the portions overlapping the main pump chamber projection area Ap. The distance X1 was 0.49 mm, which is larger than the minimum distance X1min. The left-right distance between the rear portion 79a3 and the rear portion 79b3 is constant, and this distance is set to the same as the minimum distance X1min. Therefore, the distance X2 is 0.47 mm, which is the same as the minimum distance X1min. The width of the second bent portion 77b was set to 0.33 mm. The other dimensions are the same as in Experimental Example 1, and the width Wp of the main pump chamber projected area Ap is 2 mm. Therefore, Experimental Example 11 does not satisfy either "X1 ≧ 1 / 3 × Wp" or "X2 ≧ 0.4Wp".
[0105] [Evaluation of crack occurrence rate] The crack occurrence rate was measured for each of the sensor elements of Experimental Examples 10 and 11 when the heating portion 76 was heated. Specifically, first, ten sensor elements of each of Experimental Examples 10 and 11 were prepared. Next, a constant voltage was applied to the heater 72 to heat the heating portion 76 so that the heater 72 of each sensor element reached the target temperature (800°C). Then, it was confirmed whether or not cracks occurred for each sensor element. The heating conditions were such that the heater 72 was heated to the target temperature in a shorter time than when the sensor element was normally used, so that a certain degree of cracks occurred in the sensor element. In Experimental Example 10, cracks occurred in four of the ten sensor elements, and the crack occurrence rate was 40%. In Experimental Example 11, cracks occurred in all of the ten sensor elements, and the crack occurrence rate was 100%. From these results, it was confirmed that Experimental Example 10, which satisfies both "X1 ≧ 1 / 3 × Wp" and "X2 ≧ 0.4Wp", has a lower crack occurrence rate than Experimental Example 11, which does not satisfy either "X1 ≧ 1 / 3 × Wp" or "X2 ≧ 0.4Wp". It is considered that Experimental Example 10 has a lower crack occurrence rate because it is able to reduce the stress in the internal void by satisfying both "X1 ≧ 1 / 3 × Wp" and "X2 ≧ 0.4Wp". [Explanation of symbols]
[0106] 1 first substrate layer, 2 second substrate layer, 3 third substrate layer, 4 first solid electrolyte layer, 5 spacer layer, 6 second solid electrolyte layer, 10 gas inlet, 11 first diffusion rate limiting section, 12 buffer space, 13 second diffusion rate limiting section, 20 first internal space, 21 main pump cell, 22 inner pump electrode, 22a ceiling electrode section, 22b bottom electrode section, 23 outer pump electrode, 24 variable power supply, 30 third diffusion rate limiting section, 40 second internal space, 41 measurement pump cell, 42 reference electrode, 43 reference gas introduction space, 44 measurement electrode, 46 variable power supply, 48 air introduction layer, 50 auxiliary pump cell, 51 auxiliary pump electrode, 51a ceiling electrode section, 51b bottom electrode section, 52 variable power supply, 60 fourth diffusion rate limiting section, 61 third internal space, 70 heater section, 71 heater connector electrode, 72 heater, 73 through hole, 74 heater insulating layer, 75 pressure release hole, 76 heat generating portion, 77 bent portion, 77a to 77c first to third bent portions, 78 straight portion, 78a, 78b first and second outer straight portions, 79a, 79b first and second inner straight portions, 79a1, 79b1 front portion, 79a2, 79b2 connection portion, 79a3, 79b3 rear portion, 80 oxygen partial pressure detection sensor cell for controlling main pump, 81 oxygen partial pressure detection sensor cell for controlling auxiliary pump, 82 oxygen partial pressure detection sensor cell for controlling measurement pump, 83 sensor cell, 85 lead portion, 85a, 85b first and second leads, 100 gas sensor, 101 sensor element, Am measurement chamber projected area, Ap main pump chamber projected area, Aq Auxiliary pump chamber projected area.
Claims
1. a plate-shaped element body including an oxygen ion conductive solid electrolyte layer, a measurement gas flow section for introducing and flowing a measurement gas therein, and having a longitudinal direction, a lateral direction, and a thickness direction perpendicular to the longitudinal direction and the lateral direction; a main pump cell for adjusting the oxygen concentration in a main pump chamber of the measurement gas flow section; an auxiliary pump cell that adjusts the oxygen concentration in an auxiliary pump chamber that is provided downstream of the main pump chamber in the measurement gas flow portion; a measurement pump cell for adjusting an oxygen concentration in a measurement chamber provided downstream of the auxiliary pump chamber in the measurement gas flow portion; A heating element for heating the element body; Equipped with The heating element is A first outer straight portion and a second outer straight portion are aligned along the short side direction and have a length direction along the longitudinal direction; a first inner straight portion and a second inner straight portion that are disposed between the first outer straight portion and the second outer straight portion in the short side direction and have a length direction along the longitudinal direction; a first bent portion connecting the first outer straight portion and the first inner straight portion at one end side in the longitudinal direction; a second bent portion connecting the first inner straight portion and the second inner straight portion at the other end side in the longitudinal direction; a third bent portion connecting the second inner straight portion and the second outer straight portion at one end side in the longitudinal direction; having the first inner straight portion and the second inner straight portion each at least partially overlap a main pump chamber projection area, which is an area obtained by projecting the main pump chamber in the thickness direction toward the heat generating body; the first inner straight portion and the second inner straight portion each at least partially overlap with an auxiliary pump chamber projection area, which is an area obtained by projecting the auxiliary pump chamber toward the heating element in the thickness direction, a distance X1 between the first inner straight portion and the second inner straight portion in the lateral direction at a portion where the first inner straight portion and the second inner straight portion overlap with the main pump chamber projection area is equal to or greater than ⅓ of a width Wp of the main pump chamber projection area in the lateral direction, a distance X2 between the first inner straight portion and the second inner straight portion in the short side direction at a portion where the first inner straight portion and the second inner straight portion overlap with the auxiliary pump chamber projected area is 0.4 times or more the width Wp; Sensor element.
2. The distance X1 is greater than 0.4 times the width Wp. The sensor element according to claim 1 .
3. a resistance value per unit length of a pump chamber overlapping portion, which is a portion of the heating element that overlaps with a pump chamber projection region, which is a region of the heating element where the main pump chamber and the auxiliary pump chamber are projected toward the heating element in the thickness direction, is defined as a unit resistance value R1 [μΩ / mm]; When the resistance per unit length of a measurement chamber overlapping portion, which is a portion overlapping with a measurement chamber projection area, which is an area of the heating element where the measurement chamber is projected in the thickness direction toward the heating element, is a unit resistance value R3 [μΩ / mm], The unit resistance value ratio R3 / R1 at least at any temperature in the temperature range of 700° C. or more and 900° C. or less is less than 1; The sensor element according to claim 1 or 2.
4. A gas sensor comprising the sensor element according to claim 1 or 2.
Citation Information
Patent Citations
A sensor member for detecting the proportion of gas components in the measured gas
JP2009531681A
Gas sensor
JP2012211863A
Ceramic heater, sensor element, and gas sensor
JP2017041431A
Sensor element having improved thermalproperties for determining a gas component
US20090308748A1