Negative-type photosensitive resin composition, cured film, and organic electroluminescence display device
The negative photosensitive resin composition addresses the challenges of high-definition pattern formation in organic EL devices by optimizing alkali-soluble resin formulations, achieving high light-shielding and sensitivity with reduced mask bias and improved reliability.
Patent Information
- Application Number
- JP2020143190
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-08-27
AI Technical Summary
Existing negative-tone black photosensitive resin compositions struggle to achieve high light-shielding properties and sensitivity, particularly for high-definition display applications, with significant mask bias and unreacted components affecting the long-term reliability of organic EL display devices.
A negative photosensitive resin composition containing alkali-soluble resin with specific repeating units, a polymerizable compound, a radical polymerization initiator, a colored pigment, and an organic solvent, optimized to reduce mask bias and improve long-term reliability.
The composition achieves high light-shielding properties, sensitivity, and reduced mask bias, resulting in improved pattern formation and enhanced long-term reliability of organic EL display devices.
Smart Images

Figure 0007574576000022 
Figure 0007574576000001 
Figure 0007574576000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a negative photosensitive resin composition, a cured film, and an organic electroluminescence display device. [Background technology]
[0002] 2. Description of the Related Art In recent years, many products using organic electroluminescence (hereinafter, "EL") display devices have been developed for use in thin display devices such as smartphones, tablet PCs, and televisions.
[0003] In general, an organic EL display device has a transparent electrode such as indium tin oxide (hereinafter referred to as "ITO") on the light extraction side of the light emitting element, and a metal electrode such as an alloy of magnesium and silver on the non-light extraction side of the light emitting element. In addition, an insulating layer called a pixel dividing layer is formed between the transparent electrode and the metal electrode to divide the pixels of the light emitting element.
[0004] In recent years, attempts have been made to impart light-shielding properties to pixel division layers to reduce the reflection of external light such as sunlight and improve the visibility and contrast of organic EL display devices. Specific examples of such attempts include positive-type photosensitive resin compositions using black dyes or black pigments (see, for example, Patent Documents 1 and 2) and negative-type black photosensitive resin compositions using polyimide and / or polybenzoxazole (see, for example, Patent Document 3). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6689434 [Patent Document 2] International Publication No. 2017-069172 [Patent Document 3] JP 2019-023728 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the positive type black photosensitive resin composition as in Patent Documents 1 and 2, since the black material absorbs the exposure wavelength, it is difficult to achieve both high light shielding and sensitivity, and the OD value per unit film thickness is about 0.5 at the upper limit. On the other hand, in the negative type black photosensitive resin composition as in Patent Document 3, it is possible to achieve both high light shielding and sensitivity, but in the hole pattern processing of 10 μm or less required for high-definition display applications, the absolute value of the difference between the mask design width and the hole pattern formation width (hereinafter, sometimes referred to as mask bias) becomes too large, making it difficult to form the desired pattern. Furthermore, when a cured film of a negative type black photosensitive resin composition is used in an organic EL display device, there is a problem that unreacted components remain, deteriorating the long-term reliability of the organic EL display device. [Means for solving the problem]
[0007] A negative type photosensitive resin composition comprising: an alkali-soluble resin (A) containing a repeating unit represented by general formula (1) and / or general formula (2) and a repeating unit represented by general formula (3) and / or general formula (4); a radical polymerizable compound (B); a radical polymerization initiator (C); a color pigment (D); and an organic solvent (E).
[0008] [ka]
[0009] [ka]
[0010] [ka]
[0011] [ka]
[0012] In general formula (1), R 1 represents a hydrogen atom or a methyl group, and R 2 represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkylene ether group having 1 to 5 carbon atoms and 1 oxygen atom; R 3 represents an alkyl group, an alkoxy group, or an acyl group having 1 to 5 carbon atoms. In addition, l represents an integer of 0 to 4, and m represents an integer of 1 to 4. R 3 If there are two or more R 3 may be different from each other or may be the same. In general formula (2), R 4 represents a hydrogen atom or a methyl group, and R 5 represents an alkyl group, an alkoxy group, or an acyl group having 1 to 5 carbon atoms. In addition, n represents an integer of 0 to 4, and o represents an integer of 1 to 4. 5 If there are two or more R 5 may be different from each other or may be the same. In general formula (3), R 6 represents a hydrogen atom or a methyl group, and R 7 R represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkylene ether group having 1 to 5 carbon atoms and 1 oxygen atom. 8 represents an alkyl group having 1 to 5 carbon atoms, p represents an integer of 1 to 5, and q represents an integer of 0 to 5. R 8 If there are two or more R 8 may be different from each other or may be the same. In general formula (4), R 9 represents a hydrogen atom or a methyl group, and R 10 represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkylene ether group having 1 to 5 carbon atoms and 1 oxygen atom. Effect of the Invention
[0013] According to the negative type photosensitive resin composition of the present invention, it is possible to obtain a negative type photosensitive resin composition which has both high light-shielding properties and sensitivity, has a small mask bias, and has high long-term reliability when a cured film thereof is used in an organic EL display device. [Brief description of the drawings]
[0014] [Figure 1] 1 is a schematic diagram showing a procedure for producing an organic EL display device in an example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] The present invention relates to a negative type photosensitive resin composition comprising an alkali-soluble resin (A) containing a repeating unit represented by general formula (1) and / or general formula (2) and a repeating unit represented by general formula (3) and / or general formula (4), a radically polymerizable compound (B), a radical polymerization initiator (C), a color pigment (D) and an organic solvent (E).
[0016] [ka]
[0017] [ka]
[0018] [ka]
[0019] [ka]
[0020] In general formula (1), R 1 represents a hydrogen atom or a methyl group, and R 2 represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkylene ether group having 1 to 5 carbon atoms and 1 oxygen atom; R 3 represents an alkyl group, an alkoxy group, or an acyl group having 1 to 5 carbon atoms. In addition, l represents an integer of 0 to 4, and m represents an integer of 1 to 4. R 3 If there are two or more R 3 may be different from each other or may be the same. In general formula (2), R 4 represents a hydrogen atom or a methyl group, and R 5 represents an alkyl group, an alkoxy group, or an acyl group having 1 to 5 carbon atoms. In addition, n represents an integer of 0 to 4, and o represents an integer of 1 to 4. 5 If there are two or more R 5 may be different from each other or may be the same.
[0021] In general formula (3), R 6 represents a hydrogen atom or a methyl group, and R 7 R represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkylene ether group having 1 to 5 carbon atoms and 1 oxygen atom. 8 represents an alkyl group having 1 to 5 carbon atoms, p represents an integer of 1 to 5, and q represents an integer of 0 to 5. R 8 If there are two or more R 8 may be different from each other or may be the same. In general formula (4), R 9 represents a hydrogen atom or a methyl group, and R 10 represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkylene ether group having 1 to 5 carbon atoms and 1 oxygen atom.
[0022] The negative type photosensitive resin composition of the present invention contains an alkali-soluble resin (A) (hereinafter, sometimes referred to as component (A)) containing repeating units represented by general formula (1) and / or general formula (2) and general formula (3) and / or general formula (4).
[0023] [ka]
[0024] [ka]
[0025] [ka]
[0026] [ka]
[0027] The component (A) can be obtained by copolymerizing a monomer constituting the repeating unit represented by general formula (1) and / or general formula (2) with a monomer constituting the repeating unit represented by general formula (3) and / or general formula (4). Examples of the copolymerization method include the method described in JP-A-5-19467, but any known method can also be used. Specific examples of monomers constituting the repeating unit represented by general formula (1) include 4-hydroxyphenyl methacrylate (hereinafter, PQMA), (4-hydroxyphenyl)methyl methacrylate, (4-hydroxyphenyl)ethyl methacrylate (hereinafter, PEMA), and (4-hydroxyphenyl)propyl methacrylate.
[0028] Specific examples of monomers constituting the repeating unit represented by general formula (2) include 2-hydroxystyrene, 3-hydroxystyrene, 4-hydroxystyrene, 2,4-dihydroxystyrene, 2,6-dihydroxystyrene, 2,4,6-trihydroxystyrene, 2,3,4,5-tetrahydroxystyrene, pentahydroxystyrene, 2-hydroxy-α-methylstyrene, 3-hydroxy-α-methylstyrene, 4-hydroxy-α-methylstyrene, 1-(2-hydroxyphenyl)propylene, 1-(3-hydroxyphenyl)propylene, and 1-(4-hydroxyphenyl)propylene.
[0029] By containing the repeating units represented by general formula (1) and / or general formula (2), component (A) exerts an effect of suppressing radical chain reactions, the mask bias of the negative photosensitive resin composition is reduced, and a pattern can be formed as intended. Among these, it is preferable that component (A) has a repeating unit represented by general formula (1). 2 It is more preferable that is a single bond.
[0030] In addition, examples of monomers constituting the repeating unit represented by general formula (3) include glycidyl acrylate, glycidyl methacrylate (hereinafter, sometimes referred to as GMA), 4-hydroxybutyl acrylate glycidyl ether (hereinafter, sometimes referred to as 4HBAGE), (3-ethyloxetan-3-yl)methyl acrylate, (3-methyloxetan-3-yl)methyl acrylate, (3-ethyloxetan-3-yl)methyl methacrylate, (3-methyloxetan-3-yl)methyl methacrylate, tetrahydrofurfuryl acrylate, and tetrahydro-2H-pyran-2-yl acrylate, with glycidyl methacrylate being preferred.
[0031] In addition, examples of the monomer constituting the repeating unit represented by general formula (4) include 3,4-epoxycyclohexylmethyl methacrylate, 3,4-epoxycyclohexylmethyl acrylate, 3,4-epoxycyclohexylethyl methacrylate, and 3,4-epoxycyclohexylethyl acrylate, with 3,4-epoxycyclohexylmethyl methacrylate being preferred.
[0032] When the component (A) contains a repeating unit represented by general formula (3) and / or general formula (4), the crosslink density is improved in the step of thermally curing the negative-type photosensitive resin composition after pattern processing, and an organic EL display device with excellent long-term reliability can be obtained.
[0033] When the total molar ratio of the repeating units represented by general formula (1) and the repeating units represented by general formula (2) and the total molar ratio of the repeating units represented by general formula (3) and the repeating units represented by general formula (4) are M1 and M2, respectively, relative to 100 mol% of all repeating units in component (A), it is preferable that M1 is 30 mol% or more and less than 70 mol%. By setting M1 in this range, it is possible to achieve both reduced mask bias and high sensitivity of the negative photosensitive resin composition. From the viewpoints of storage stability of the negative photosensitive resin composition and minimizing mask bias, the ratio of M1 / M2 is preferably 0.4 or more, and more preferably 0.6 or more, while from the viewpoint of long-term reliability of the organic EL display device, the ratio of M1 / M2 is preferably 1.5 or less.
[0034] Component (A) can further be copolymerized with any (meth)acrylic monomer as a monomer, if necessary. Specifically, monomers having a carboxy group, such as acrylic acid, methacrylic acid, itaconic acid, maleic acid, maleic anhydride, phthalic acid, phthalic anhydride, crotonic acid, 2-carboxyethyl acrylate oligomer, 2-carboxyethyl methacrylate oligomer, etc., methyl acrylate, ethyl acrylate, propyl acrylate, isopropyl acrylate, n-butyl acrylate, isobutyl acrylate, t-butyl acrylate, cyclohexyl acrylate, isobornyl acrylate, benzyl acrylate, 2-ethylhexyl acrylate, ethyl methacrylate, propyl methacrylate, isopropyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, etc. and acrylic esters or methacrylic esters, such as butyl methacrylate, t-butyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, benzyl methacrylate, 2-ethylhexyl methacrylate, or (fluoro)alkyl ester monomers thereof; and unsaturated monomers having an aromatic ring, such as styrene, α-methylstyrene, 4-vinyltoluene and its structural isomers, 4-methoxystyrene and its structural isomers, 4-butoxystyrene and its structural isomers, 4-tert-butoxystyrene and its structural isomers, 4-vinylbiphenyl, 2-vinylnaphthalene and its structural isomers, 9-vinylanthracene, and 9-vinylcarbazole.
[0035] The content of the component (A) in the negative photosensitive resin composition is preferably 5 parts by weight or more, more preferably 10 parts by weight or more, based on 100 parts by weight of the total of the components other than the solvent in the negative photosensitive resin composition, from the viewpoint of minimizing mask bias. On the other hand, the content of the component (A) is preferably 60 parts by weight or less, more preferably 50 parts by weight or less, based on 100 parts by weight of the total of the components other than the solvent in the negative photosensitive resin composition, from the viewpoint of improving the sensitivity during exposure.
[0036] The negative photosensitive resin composition contains a radical polymerizable compound (B) (hereinafter, may be referred to as component (B)). Here, the solvent refers to the organic solvent (E) and water.
[0037] From the viewpoint of improving the sensitivity during exposure, the radical polymerizable group of the (B) component is preferably an acrylic group or a methacrylic group, and two kinds of these may be contained. The (B) component is preferably a compound having two or more radical polymerizable groups. Examples of the (B) component include bisphenol A diglycidyl ether (meth)acrylate, poly(meth)acrylate carbamate, modified bisphenol A epoxy (meth)acrylate, adipic acid 1,6-hexanediol (meth)acrylic acid ester, phthalic anhydride propylene oxide (meth)acrylic acid ester, trimellitic acid diethylene glycol (meth)acrylic acid ester, rosin modified epoxy di(meth)acrylate, alkyd modified (meth)acrylate, fluorene diacrylate oligomer, tripropylene glycol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, bisphenol A diglycidyl ether Di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, triacrylformal, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, 2,2-bis[4-(3-acryloxy-2-hydroxypropoxy)phenyl]propane, bis[4-(3-acryloxy-2-hydroxypropoxy)phenyl]methane, bis[4-(3-acryloxy-2-hydroxypropoxy)phenyl]sulfone, bis[4-(3-acryloxy-2-hydroxypropoxy)phenyl]ether, 4,4' 9,9-bis[4-(3-acryloxy-2-hydroxypropoxy)phenyl]cyclohexane, 9,9-bis[4-(3-acryloxy-2-hydroxypropoxy)phenyl]fluorene, 9,9-bis[3-methyl-4-(3-acryloxy-2-hydroxypropoxy)phenyl]fluorene, 9,9-bis[3-chloro-4-(3-acryloxy-2-hydroxypropoxy)phenyl]fluorene, bisphenoxyethanol fluorene diacrylate, bisphenoxyethanol fluorene dimethacrylate, biscresol fluorene diacrylate, and biscresol fluorene dimethacrylate.Two or more of these may be contained. From the viewpoint of further improving the sensitivity, a compound having three or more radical polymerizable groups is more preferable, a compound having five or more radical polymerizable groups is more preferable, and dipentaerythritol hexa(meth)acrylate and dipentaerythritol penta(meth)acrylate are further preferable.
[0038] The content of the component (B) in the negative photosensitive resin composition is preferably 10 parts by weight or more, and more preferably 15 parts by weight or more, per 100 parts by weight of the total content of the components (A) and (B) from the viewpoint of improving sensitivity during exposure. On the other hand, the content of the component (B) is preferably 80 parts by weight or less, and more preferably 60 parts by weight or less, per 100 parts by weight of the total content of the alkali-soluble resin (A) and the radically polymerizable compound (B), from the viewpoint of reflowability in the heating and baking step.
[0039] The negative photosensitive resin composition contains a radical polymerization initiator (C) (hereinafter, may be referred to as component (C)).
[0040] The component (C) refers to a compound that generates radicals by bond cleavage and / or reaction upon exposure. Examples include carbazole-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, oxime ester-based photopolymerization initiators, and α-aminoalkylphenone-based photopolymerization initiators. Two or more of these may be contained. Among these, carbazole-based photopolymerization initiators and oxime ester-based photopolymerization initiators are preferred because they have high sensitivity to a mixed line consisting of i-line (365 nm), h-line (405 nm), and g-line (436 nm) in the exposure step described below.
[0041] The content of the component (C) in the negative photosensitive resin composition is preferably 1 part by weight or more, more preferably 5 parts by weight or more, per 100 parts by weight of the radical polymerizable compound (B) from the viewpoint of improving sensitivity to light exposure, while the content of the component (C) is preferably 60 parts by weight or less, more preferably 40 parts by weight or less, per 100 parts by weight of the radical polymerizable compound (B) from the viewpoint of fine line processability.
[0042] The negative photosensitive resin composition contains a color pigment (D) (hereinafter, may be referred to as component (D)).
[0043] As the component (D), organic pigments and inorganic pigments generally used in the field of electronic information materials can be used. Examples of organic pigments include diketopyrrolopyrrole pigments, azo pigments such as azo, disazo, or polyazo, phthalocyanine pigments such as copper phthalocyanine, halogenated copper phthalocyanine, or metal-free phthalocyanine, anthraquinone pigments such as aminoanthraquinone, diaminodianthraquinone, anthrapyrimidine, flavanthrone, anthanthrone, indanthrone, pyranthrone, or violanthrone, quinacridone pigments, dioxazine pigments, perinone pigments, perylene pigments, thioindigo pigments, isoindoline pigments, isoindolinone pigments, quinophthalone pigments, threne pigments, or metal complex pigments.
[0044] Examples of inorganic pigments include titanium oxide, zinc oxide, zinc sulfide, white lead, calcium carbonate, precipitated barium sulfate, white carbon, alumina white, kaolin clay, talc, bentonite, black iron oxide, cadmium red, red iron oxide, molybdenum red, molybdate orange, chrome vermilion, yellow lead, cadmium yellow, yellow iron oxide, titanium yellow, chromium oxide, viridian, titanium cobalt green, cobalt green, cobalt chrome green, Victoria green, ultramarine, Prussian blue, cobalt blue, cerulean blue, cobalt silica blue, cobalt zinc silica blue, manganese violet, and cobalt violet.
[0045] Examples of red pigments include Pigment Red 9, 48, 97, 122, 123, 144, 149, 166, 168, 177, 179, 180, 192, 209, 215, 216, 217, 220, 223, 224, 226, 227, 228, 240, and 254 (all numbers are Color Index (hereinafter, "CI" numbers)).
[0046] Examples of orange pigments include Pigment Orange 13, 36, 38, 43, 51, 55, 59, 61, 64, 65, and 71.
[0047] Examples of yellow pigments include Pigment Yellow 12, 13, 17, 20, 24, 83, 86, 93, 95, 109, 110, 117, 125, 129, 137, 138, 139, 147, 148, 150, 153, 154, 166, 168, and 185 (all numbers are CI numbers).
[0048] Examples of purple pigments include Pigment Violet 19, 23, 29, 30, 32, 37, 40, and 50 (all numbers are CI numbers).
[0049] Examples of blue pigments include Pigment Blue 15, 15:3, 15:4, 15:6, 22, 60, and 64 (all numbers are CI numbers).
[0050] Examples of green pigments include Pigment Green 7, 10, 36, and 58 (all numbers are CI numbers).
[0051] Examples of black pigments include black organic pigments, mixed-color organic pigments, inorganic pigments, etc. Examples of black organic pigments include carbon black, perylene black, aniline black, and benzofuranone pigments (described in JP-T 2012-515233).
[0052] Although a negative photosensitive resin composition having desired optical properties can be obtained by combining these color pigments, it is preferable to include a benzofuranone pigment from the viewpoints of visible light shielding property and insulating property per unit weight.
[0053] The content of the component (D) in the negative photosensitive resin composition is preferably 5 parts by weight or more, more preferably 10 parts by weight or more, relative to 100 parts by weight of the total solid content of the negative photosensitive resin composition, from the viewpoint of light-shielding property per unit film thickness. On the other hand, the content of the component (D) is preferably 50 parts by weight or less, more preferably 40 parts by weight or less, relative to 100 parts by weight of the negative photosensitive resin composition, from the viewpoint of improving sensitivity during exposure and fine line processability.
[0054] The negative photosensitive resin composition contains an organic solvent (E) (hereinafter, may be referred to as component (E)).
[0055] Examples of the component (E) include ethers, acetates, esters, ketones, aromatic hydrocarbons, amides, and alcohols.
[0056] Examples of the ethers include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, tetrahydrofuran, etc. Examples of the acetates include ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, 3-methoxybutyl acetate, diethylene glycol monomethyl ether acetate, propylene glycol monomethyl ether acetate (hereinafter, "PGMEA"), propylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, etc. Examples of esters include methyl 2-hydroxypropionate, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, 3-methoxybutyl acetate, ethyl acetate, n-propyl acetate, n-butyl acetate, etc. Examples of ketones include methyl ethyl ketone, cyclohexanone, 2-heptanone, 3-heptanone, etc. Examples of aromatic hydrocarbons include toluene and xylene, etc. Examples of amides include N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, etc. Examples of alcohols include butyl alcohol, isobutyl alcohol, pentanol, 4-methyl-2-pentanol, 3-methyl-2-butanol, 3-methyl-3-methoxybutanol, diacetone alcohol, etc. Two or more of these may be contained. Among these, the boiling point at 1 atmospheric pressure is preferably 170° C. or less, and more preferably 150° C. or less, since the solvent is easily volatilized even when low-temperature baking is performed after patterning.
[0057] The negative type photosensitive resin composition may further contain a resin (F) (hereinafter sometimes referred to as component (F)) having a repeating unit represented by general formula (5) having a tertiary amino group in a side chain, a repeating unit having a carboxy group, and a repeating unit having an ethylenically unsaturated group.
[0058] [ka]
[0059] In general formula (5), R 11 represents a hydrogen atom or a methyl group, and R 12 R represents a single bond, an alkyl group having 1 to 5 carbon atoms, or an alkylene ether group having 1 to 5 carbon atoms and 1 oxygen atom. 13 , R 14 each independently represents an alkyl group or alkoxy group having 1 to 5 carbon atoms, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, or an aromatic hydrocarbon group having 6 to 10 carbon atoms.
[0060] Specific examples of monomers constituting the repeating unit represented by general formula (5) include 2-dimethylaminoethyl acrylate, 2-diethylaminoethyl acrylate, 2-dipropylaminoethyl acrylate, 2-diphenylaminoethyl acrylate, 2-dibenzylaminoethyl acrylate, 2-dimethylaminoethyl methacrylate, 2-diethylaminoethyl methacrylate, 2-dipropylaminoethyl methacrylate, 2-diphenylaminoethyl methacrylate, and 2-benzylaminoethyl methacrylate. These monomers may be used alone or in combination of two or more. By including an alkali-soluble resin having a repeating unit represented by general formula (5), a tertiary amino group is adsorbed on the color pigment surface, and the storage stability of the negative photosensitive resin composition can be further improved.
[0061] Specific examples of monomers constituting the repeating unit having a carboxy group include acrylic acid, methacrylic acid, itaconic acid, maleic acid, maleic anhydride, phthalic acid, phthalic anhydride, crotonic acid, 2-carboxyethyl acrylate oligomer, and 2-carboxyel methacrylate oligomer.
[0062] As a method for synthesizing the component (F), a method can be used in which a structural unit represented by the general formula (5) and a carboxyl group-containing unit are polymerized, and then a repeating unit having a known ethylenically unsaturated group is introduced. For example, a method can be used in which a glycidyl group-containing polymerizable unsaturated monomer is subjected to an addition reaction with a (meth)acrylic copolymer obtained by copolymerizing a carboxyl group-containing unsaturated monomer. In this case, examples of the carboxyl group-containing unsaturated monomer to be copolymerized include acrylic acid and methacrylic acid, and examples of the glycidyl group-containing unsaturated monomer to be copolymerized include glycidyl acrylate and glycidyl methacrylate. These acrylic monomers can be used alone or in a mixture of two or more kinds.
[0063] The acid value of the (F) component is preferably 50 to 120 mgKOH / g, and by setting it in this range, it is possible to achieve both color pigment dispersion stability and solubility in an alkaline developer. The base number is preferably 5 to 70 mmol / 100 g, and by setting it in this range, it is possible to improve the color pigment dispersion stability while maintaining solubility in an alkaline developer. The base number is defined as the number of moles of perchloric acid required to neutralize 100 g of the (F) component.
[0064] From the viewpoint of color pigment dispersion stability, the content of component (F) is preferably 5 parts by weight or more per 100 parts by weight of components (A) and (F) combined, while from the viewpoint of minimizing mask bias, the content of component (F) is preferably 50 parts by weight or less per 100 parts by weight of components (A) and (F) combined.
[0065] The negative photosensitive resin composition may contain a surfactant for the purpose of improving wettability with the substrate or improving the thickness uniformity of the photosensitive resin film as necessary. Commercially available compounds can be used as the surfactant. Specifically, silicone surfactants include the SH series, SD series, and ST series of Toray Dow Corning Silicone, the BYK series of BYK Japan, the KP series of Shin-Etsu Silicone, the Disform series of Nippon Oil & Fats, and the TSF series of Toshiba Silicone. Fluorine-based surfactants include the "Megafac (registered trademark)" series of Dainippon Ink & Coatings, the Fluorard series of Sumitomo 3M, the "Surflon (registered trademark)" series and "Asahi Guard (registered trademark)" series of Asahi Glass, the EF series of Shin-Akita Chemical, and the Polyfox series of OmNova Solutions. Surfactants made of acrylic and / or methacrylic polymers include the Polyflow series of Kyoeisha Chemical, and the "Disparon (registered trademark)" series of Kusumoto Chemical, but are not limited thereto.
[0066] The content of the surfactant is preferably 0.0001 part by weight or more and 1 part by weight or less based on 100 parts by weight of the negative photosensitive resin composition.
[0067] The negative photosensitive resin composition may contain a polymer dispersant. The polymer dispersant refers to a dispersant having both an affinity group having a chemical bond or adsorption action to the color pigment surface and a polymer chain or group having solvent affinity, and is different from the component (F) in that it does not contain an ethylenically unsaturated group. Since the polymer dispersant does not have an ethylenically unsaturated group, there is a concern that the target photosensitive performance may be deteriorated if it is added in a large amount, and it is desirable to add an appropriate amount taking into account the dispersion stability and photosensitive performance. In the wet media dispersion treatment described later, the polymer dispersant improves the wettability of the color pigment to the dispersion medium to promote the deaggregation of the light-shielding material, stabilizes the particle size and viscosity by steric hindrance and / or electrostatic repulsion effect, and further has the effect of suppressing the occurrence of color separation during storage or application of the negative photosensitive resin composition.
[0068] Examples of the polymer dispersant include polyester-based polymer dispersants, acrylic-based polymer dispersants, polyurethane-based polymer dispersants, polyallylamine-based polymer dispersants, carbodiimide-based dispersants, etc. Among these, polymer dispersants having an amino group are preferred in order to improve the long-term storage stability of the color pigment dispersion.
[0069] Examples of methods for producing a negative type photosensitive resin composition include a method in which the component (D) is directly dispersed in a solution containing the components (A), (B), and (C) using a disperser, and a method in which the component (D) is dispersed in the component (A) using a disperser to prepare a colored dispersion, and then the colored dispersion is mixed with the components (B) and (C).
[0070] Examples of the dispersing machine include a ball mill, a sand grinder, a three-roll mill, and a high-speed impact mill. Among these, a bead mill is preferred from the viewpoint of improving dispersion efficiency and fine dispersion. Examples of the bead mill include a coball mill, a basket mill, a pin mill, and a dyno mill. Examples of the beads of the bead mill include titania beads, zirconia beads, and zircon beads. The bead diameter of the bead mill is preferably 0.03 to 1.0 mm. When the primary particle diameter of the component (A) and the particle diameter of the secondary particles formed by aggregation of the primary particles are small, minute dispersion beads of 0.03 to 0.10 mm are preferred.
[0071] In this case, a bead mill having a separator using a centrifugal separation method capable of separating minute beads from the dispersion liquid is preferred. On the other hand, when dispersing component (D) containing coarse particles of the submicron order, beads with a bead diameter of 0.10 mm or more are preferred because they provide sufficient crushing power. The bead diameter can be calculated by measuring the circle equivalent diameter of 100 beads randomly selected by microscopic observation and calculating the number average value.
[0072] The cured film of the present invention is obtained by curing the negative photosensitive resin composition. Methods for curing the negative photosensitive resin composition include photocuring and heat curing. Specifically, it is preferable to carry out both photocuring and heat curing, which will be described later.
[0073] A method for producing a cured film obtained by curing a negative photosensitive resin composition will be described below.
[0074] The method for producing the cured film includes a step of applying a negative photosensitive resin composition to form a photosensitive resin film, a step of drying the photosensitive resin film, a step of exposing the photosensitive resin film, a step of developing the exposed photosensitive resin film, and a step of heat curing. Specific methods for producing the cured film include, for example, the method described in JP-A-2019-023728, but the film can also be produced by known methods.
[0075] The organic EL display device of the present invention comprises the cured film. The organic EL display device has at least a substrate, a first electrode, a second electrode, a light-emitting pixel, a planarization layer, and a pixel division layer. An active matrix type organic EL display device having a plurality of pixels formed in a matrix is preferred. The active matrix type display device has light-emitting pixels on a substrate such as glass, and has a planarization layer provided so as to cover the lower parts of the light-emitting pixels and parts other than the light-emitting pixels. Furthermore, on the planarization layer, there is a first electrode provided so as to cover at least the lower parts of the light-emitting pixels, and a second electrode provided so as to cover at least the upper parts of the light-emitting pixels. In addition, the active matrix type display device has an insulating pixel division layer to divide the light-emitting pixels, and the cured film obtained from the negative type photosensitive resin composition of the present invention can be suitably used for the pixel division layer.
[0076] In addition, since the negative type photosensitive resin composition of the present invention is capable of forming a high-definition pattern that does not leave residues in the openings, it can also be used for colored partitions for solid-state imaging elements, micro LEDs, and mini LED display devices, and black matrices and black column spacers used in color filters for liquid crystal display devices. EXAMPLES
[0077] The present invention will be described in detail below with reference to examples and comparative examples, but the aspects of the present invention are not limited to these.
[0078] <Evaluation method> [Molecular weight] The weight average molecular weight (Mw) was measured using gel permeation chromatography (GPC) "HLC-8220GPC" (a testing device manufactured by Tosoh Corporation) with tetrahydrofuran as a carrier and polystyrene as a molecular weight standard.
[0079] [sensitivity] The negative photosensitive resin compositions obtained in each of the Examples and Comparative Examples were applied onto an ITO substrate using a spinner (MS-A150) manufactured by Mikasa Co., Ltd., so that the OD value of the photosensitive resin film was 1.5, and the photosensitive resin film was heated and dried on a hot plate at 100°C for 2 minutes. This photosensitive resin film was irradiated with 500 mJ / cm2 of a high-pressure mercury lamp as a light source using a mask aligner (PEM-6M) manufactured by Union Optical Co., Ltd., through a negative mask (stripe design line width 10 μm) manufactured by HOYA Co., Ltd. 2 The maximum exposure is 10 mJ / cm 2 The exposure dose was reduced for each exposure, and the patterned substrate was developed for 60 seconds with an alkaline developer of 2.38 wt% TMAH aqueous solution to obtain a patterned substrate. The patterned substrate was then baked in a hot air oven at 230°C for 60 minutes to obtain a cured film.
[0080] The cured film of the obtained negative photosensitive resin composition was observed under an optical microscope, and the minimum exposure dose (mJ / cm) at which the cured film could be formed without peeling was determined. 2 ) was defined as the sensitivity. [Light blocking property] Of the cured films of the negative type photosensitive resin compositions obtained in each of the Examples and Comparative Examples, the OD value of the cured film at the minimum exposure dose at which a pattern could be formed was measured using an X-rite 361T (visual) densitometer to measure the intensities of incident light and transmitted light, and calculated using the following formula (3).
[0081] OD value=log 10 (I0 / I) Equation (3) I0: Incident light intensity I: transmitted light intensity In addition, the thickness of the cured film was measured using a contact type film thickness meter DEKTAK150 (manufactured by ULVAC, Inc.), and the light blocking ability per 1 μm of each cured film was evaluated by calculating the OD value / film thickness.
[0082] [Mask Bias] Of the cured films of the negative photosensitive resin compositions obtained in each of the Examples and Comparative Examples, the opening width of a stripe pattern with a mask opening width of 10 μm at the minimum exposure dose that enabled pattern formation was measured using an optical microscope, and it was determined that the smaller the absolute value of the difference between the mask design value and the opening width of the cured film, the smaller the mask bias and the better the result.
[0083] evaluation A: Mask bias less than 1.0 μm B: Mask bias 1.0μm or more and less than 2.0μm C: Mask bias 2.0μm or more and less than 3.0μm D: Mask bias 3.0 μm or more.
[0084] [Storage stability] The initial sensitivity of the negative photosensitive resin compositions obtained in the Examples and Comparative Examples and the sensitivity after standing for 7 days at 23° C. were evaluated in the same manner as for the initial sensitivity. A smaller sensitivity change rate (%), which is the ratio of the sensitivity after aging to the initial sensitivity, was determined to be a negative photosensitive resin composition with excellent stability.
[0085] evaluation A: Sensitivity change rate less than 120% B: Sensitivity change rate 120% or more, less than 150% C: Sensitivity change rate 150% or more, less than 200% D: Sensitivity change rate is 200% or more.
[0086] [Long-term reliability evaluation of organic electroluminescence display devices] FIG. 1 shows a schematic diagram of the procedure for producing an organic EL display device using the negative photosensitive resin composition obtained in each Example and Comparative Example. First, a 10 nm ITO transparent conductive film was formed on the entire surface of a 38 mm x 46 mm alkali-free glass substrate 1 by sputtering, and etched as a first electrode (transparent electrode) 2. At the same time, an auxiliary electrode 3 for extracting a second electrode was also formed. The obtained substrate was ultrasonically cleaned with Semicoclean 56 (trade name, manufactured by Furuuchi Chemical Co., Ltd.) for 10 minutes, and then washed with ultrapure water. Next, a negative photosensitive resin composition (PB-1) was applied to the entire surface of the substrate by spin coating, and prebaked on a hot plate at 100 ° C. for 2 minutes. This film was exposed to light through a photomask with a high-pressure mercury lamp as a light source at the minimum exposure amount of each negative photosensitive resin composition, and then developed with a 2.38 wt % TMAH aqueous solution, unnecessary parts were dissolved, and rinsed with pure water. The obtained resin pattern was heat-treated in a hot air oven at 230 ° C. for 60 minutes. In this way, an insulating layer 4 was formed in a limited area of the substrate, in which openings 70 μm wide and 260 μm long were arranged at a pitch of 155 μm in the width direction and a pitch of 465 μm in the length direction, and each opening had a shape that exposed the first electrode. In this way, an insulating layer with an insulating layer aperture ratio of 25% was formed in the substrate effective area, which was a rectangle with one side of 16 mm. The thickness of the insulating layer was about 1.0 μm.
[0087] Next, a nitrogen plasma treatment was performed as a pretreatment, and then an organic EL layer 5 including a light-emitting layer was formed by a vacuum deposition method. Note that the degree of vacuum during deposition was 1×10 -3 The pressure was below 10 Pa, and the substrate was rotated relative to the deposition source during deposition. First, compound (HT-1) was deposited to a thickness of 10 nm as a hole injection layer, and compound (HT-2) was deposited to a thickness of 50 nm as a hole transport layer. Next, compound (GH-1) as a host material and compound (GD-1) as a dopant material were deposited to a thickness of 40 nm in the light-emitting layer so that the doping concentration was 10%. Next, compound (ET-1) and compound (LiQ) were laminated to a thickness of 40 nm in a volume ratio of 1:1 as electron transport materials. The structures of the compounds used in the organic EL layer are shown below.
[0088] [ka]
[0089] Next, a compound (LiQ) was evaporated to a thickness of 2 nm, and then Mg and Ag were evaporated to a thickness of 10 nm at a volume ratio of 10:1 to form a second electrode (non-transparent electrode) 6. Finally, a cap-shaped glass plate was attached to the substrate in a low-humidity nitrogen atmosphere using an epoxy resin adhesive to seal the substrate, and four top-emission organic EL display devices, each of which was a rectangle with a side length of 5 mm, were fabricated on one substrate. The film thickness referred to here is the value displayed on a quartz crystal oscillator film thickness monitor. The fabricated organic EL display device was placed on a hot plate heated to 80°C with the light-emitting surface facing up, and was illuminated with a wavelength of 365 nm and an illuminance of 0.6 kmW / cm. 2 The organic EL display device was driven with a direct current of 0.625 mA to emit light, and the area ratio of the light-emitting portion to the area of the light-emitting pixel (pixel light-emitting area ratio) was measured immediately after irradiation (0 hours) and after 1000 hours had elapsed. If the pixel light-emitting area ratio after 1000 hours using this evaluation method is 80% or more, it can be said to have excellent long-term reliability, and if it is 90% or more, it is more preferable.
[0090] evaluation A: Pixel light-emitting area ratio 95% or more B: Pixel light-emitting area ratio: 90% or more, less than 95% C: Pixel light-emitting area ratio: 80% or more, less than 90% D: Pixel light-emitting area ratio is less than 80%.
[0091] <Production Example> (Synthesis Example 1: Alkali-soluble resin A-1) 33.40g of 4-hydroxyphenyl methacrylate ("PQMA" manufactured by Showa Denko K.K.) and 6.66g of GMA were completely dissolved in 100.0g of PGMEA, and 3.66g of V-601 (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) as a polymerization initiator was completely dissolved in 15.0g of PGMEA. The two obtained solutions were simultaneously dropped into 45.0g of PGMEA heated to 85°C under a nitrogen gas atmosphere in a 300mL three-neck flask over a period of 2 hours, and after completion of the dropping, the mixture was reacted at 85°C for 3 hours to obtain a 20% by weight solids solution of alkali-soluble resin A-1 with PQMA / GMA=80 / 20. The weight-average molecular weight of the obtained reaction product was 8800.
[0092] (Synthesis Example 2: Alkali-soluble resin A-2) A 20 wt% solids solution of alkali-soluble resin A-2 (PQMA / GMA=70 / 30) was obtained by changing the amount of PQMA to 29.80 g and the amount of GMA to 10.20 g in the same manner as in Synthesis Example 1. The weight average molecular weight of the resulting reaction product was 8,500.
[0093] (Synthesis Example 3: Alkali-soluble resin A-3) A 20% by weight solids solution of alkali-soluble resin A-3 (PQMA / GMA=60 / 40) was obtained by changing the amount of PQMA to 26.10 g and the amount of GMA to 13.90 g in the same manner as in Synthesis Example 1. The weight average molecular weight of the resulting reaction product was 8,600.
[0094] (Synthesis Example 4: Alkali-soluble resin A-4) A 20 wt% solids solution of alkali-soluble resin A-4 (PQMA / GMA=40 / 60) was obtained by changing the amount of PQMA to 18.20 g and the amount of GMA to 21.80 g in the same manner as in Synthesis Example 1. The weight average molecular weight of the resulting reaction product was 8,300.
[0095] (Synthesis Example 5: Alkali-soluble resin A-5) A 20 wt% solids solution of alkali-soluble resin A-5 (PQMA / GMA=35 / 65) was obtained by changing the amount of PQMA to 16.11 g and the amount of GMA to 23.89 g in the same manner as in Synthesis Example 1. The weight average molecular weight of the resulting reaction product was 8,100.
[0096] (Synthesis Example 6: Alkali-soluble resin A-6) A 20% by weight solids solution of alkali-soluble resin A-6 (PQMA / GMA=30 / 70) was obtained by changing the amount of PQMA to 13.97 g and the amount of GMA to 26.03 g in the same manner as in Synthesis Example 1. The weight average molecular weight of the resulting reaction product was 8,400.
[0097] (Synthesis Example 7: Alkali-soluble resin A-7) A 20% by weight solids solution of alkali-soluble resin A-7 (PQMA / GMA=20 / 80) was obtained by changing the amount of PQMA to 9.54 g and the amount of GMA to 30.46 g in the same manner as in Synthesis Example 1. The weight average molecular weight of the resulting reaction product was 8,400.
[0098] (Synthesis Example 8: Alkali-soluble resin A-8) A 20% by weight solids solution of alkali-soluble resin A-8 (PEMA / GMA=20 / 80) was obtained by using PEMA instead of PQMA and changing the amount of PEMA and GMA to 10.64g and 29.36g, respectively, in the same manner as in Synthesis Example 1. The weight average molecular weight of the reaction product obtained was 8,800.
[0099] (Synthesis Example 9: Alkali-soluble resin A-9) A 20% by weight solids solution of alkali-soluble resin A-9 with a ratio of 4-hydroxystyrene / GMA=20 / 80 was obtained by using 4-hydroxystyrene instead of PQMA as the monomer type added in the same manner as in Synthesis Example 1, and changing the amount of 4-hydroxystyrene to 6.97g and the amount of GMA to 33.03g. The weight average molecular weight of the reaction product obtained was 9000.
[0100] (Synthesis Example 10: Alkali-soluble resin A-10) A 20 wt% solids solution of alkali-soluble resin A-10 (PQMA / 4HBAGE=40 / 60) was obtained by using 4HBAGE instead of GMA as the monomer type added in the same manner as in Synthesis Example 1, and changing the amount of PQMA to 14.90 g and the amount of 4HBAGE to 25.10 g. The weight-average molecular weight of the resulting reaction product was 8,100.
[0101] (Synthesis Example 11: Alkali-soluble resin A-11) The same method as in Synthesis Example 1 was used, but instead of GMA, (3-ethyloxetan-3-yl)methyl methacrylate (OXE-30, manufactured by Osaka Organic Chemical Industry Co., Ltd.) was used as the monomer, and the amount of PQMA was 17.08 g and the amount of OXE-30 was 22.92 g, to obtain a 20 wt % solids solution of alkali-soluble resin A-11 with a PQMA / OXE-30 ratio of 40 / 60. The weight-average molecular weight of the resulting reaction product was 9,200.
[0102] (Synthesis Example 12: Alkali-soluble resin A-12) A 20 wt% solids solution of alkali-soluble resin A-12 (PQMA=100) was obtained by changing the type of monomer added to only 40.00 g of PQMA in the same manner as in Synthesis Example 1. The weight average molecular weight of the resulting reaction product was 7,500.
[0103] (Synthesis Example 13: Alkali-soluble resin A-13) A 20 wt% solids solution of alkali-soluble resin A-13 with GMA=100 was obtained by changing the type of monomer added to only 40.00 g of GMA in the same manner as in Synthesis Example 1. The weight average molecular weight of the resulting reaction product was 8,800.
[0104] (Synthesis Example 14: Tertiary Amino Group and Ethylenically Unsaturated Group-Containing Resin (F-1)) 400.0g of PGMEA was charged into a pressure vessel equipped with a stirrer, thermometer, reflux condenser, and dropping pump, and the inside of the reaction vessel was filled with nitrogen, then the temperature was raised to 90°C, and a mixture of 2.0g of 2-dimethylaminoethyl methacrylate, 31.0g of methyl methacrylate, 20.0g of 2-ethylhexyl methacrylate, 30.0g of styrene, 17.0g of methacrylic acid, 2.0g of azobisisobutyronitrile as a polymerization initiator, and 3.0g of normal dodecyl mercaptan was dropped into the vessel over 3 hours using a dropping pump to carry out copolymerization. After that, the inside of the reaction vessel was replaced with air, and 10.0g of GMA was dropped into the vessel over 1 hour using a dropping pump to carry out an addition reaction, and the vessel was stirred for another 2 hours. As a result, a tertiary amino group- and ethylenically unsaturated group-containing resin (F-1) solution with a solid content of 20% by weight and characteristic values of a base number of 11 mmol / 100 g, an acid value of 73 mg KOH / g, and a weight average molecular weight of 7,000 was obtained.
[0105] (Synthesis Example 15: Resin (DP-1) that does not fall under either component (A) or component (F)) Using the method described in the literature (Japanese Patent No. 3120476, Example 1), a methyl methacrylate / methacrylic acid / styrene copolymer (weight ratio 30 / 40 / 30) was synthesized, and then 40 parts by weight of GMA was added thereto. The copolymer was then reprecipitated in purified water, filtered, and dried to obtain an acrylic copolymer (DP-1) with a weight average molecular weight (Mw) of 10,000 and an acid value of 110 (mgKOH / g).
[0106] (Production Example 1: Production of Color Pigment Dispersion (DB-1)) 600 g of Irgaphor Black S0100CF (manufactured by BASF) as a color pigment, 468.5 g of a 20 wt% PGMEA solution of a resin (F-1) having a tertiary amino group, and 56.3 g of a dispersant having an amine value of 20 mgKOH / g described in Synthesis Example 2 of JP-A-2020-070352 and 1875.2 g of PGMEA as a polymer dispersant were charged into a tank and stirred with a homomixer for 20 minutes to obtain a preliminary dispersion. The obtained preliminary dispersion was supplied to a dispersing machine Ultra Apex Mill manufactured by Hiroshima Metal & Machinery Co., Ltd. equipped with a centrifugal separator filled with 70% by volume of 0.10 mmφ zirconia beads, and dispersion was performed at a rotation speed of 10 m / s for 3 hours to obtain a color pigment dispersion (DB-1) with a solid content concentration of 25 wt% and color pigment / resin (by weight) = 80 / 20.
[0107] (Production Example 2: Production of Color Pigment Dispersion (DB-2)) A color pigment dispersion (DB-2) with a solid concentration of 25% by weight and color pigment / resin (by weight) = 80 / 20 was obtained by the same manufacturing method as DB-1, except that a 20% by weight solution of resin (DP-1) in PGMEA was used.
[0108] Example 1 To 180.9 g of color pigment dispersion (DB-1), 284.3 g of 20 wt% PGMEA solution of alkali-soluble resin (A-1), 5.3 g of Adeka Arcles (registered trademark) NCI-831 as a photopolymerization initiator, 42.4 g of dipentaerythritol hexaacrylate (manufactured by Nippon Kayaku Co., Ltd.) as a radical polymerizable compound, 0.2 g of silicone surfactant "BYK" (registered trademark) 333 (manufactured by BYK Chemie Co., Ltd.), and 486.9 g of PGMEA were added to obtain a negative type photosensitive resin composition (PB-1) with a total solid concentration of 15 wt% and a color pigment / resin (weight ratio) of 25 / 75. Furthermore, a cured film of the obtained negative type photosensitive resin composition and an organic EL display device having the cured film were prepared according to the above-mentioned method.
[0109] (Examples 2 to 11) In the same manner as in Example 1, negative-type photosensitive resin compositions (PB-2) to (PB-11), cured films thereof, and organic EL display devices equipped with the cured films were obtained by using A-2 to A-10 as the alkali-soluble resins to be added, respectively.
[0110] Example 12 In the same manner as in Example 1, DB-2 was used as the color pigment dispersion and A-4 was used as the alkali-soluble resin to be added, thereby obtaining a negative type photosensitive resin composition (PB-12), a cured film thereof, and an organic EL display device having the cured film thereof.
[0111] (Comparative Examples 1 to 3) In the same manner as in Example 12, negative-type photosensitive resin compositions (PB-13) to (PB-15), cured films thereof, and organic EL display devices using these compositions as insulating layers were obtained by using A-12, A-13, and DP-1, respectively, as the alkali-soluble resins to be added. The compositions of the examples and comparative examples are shown in Table 1, and the evaluation results are shown in Table 2.
[0112] [Table 1]
[0113] [Table 2]
[0114] The negative type photosensitive resin compositions of the Examples achieved both high light-shielding properties and sensitivity, while reducing the mask bias during fine pattern processing. In addition, they had excellent storage stability as negative type photosensitive resin compositions, and the organic EL display devices using the cured films thereof had excellent long-term reliability. On the other hand, the negative photosensitive resin compositions of the comparative examples, Comparative Example 1 containing the homopolymer of general formula (1), had good mask bias but poor long-term reliability of the organic EL display device using the cured film, and Comparative Example 2 containing the homopolymer of general formula (3) had poor storage stability as a negative photosensitive resin composition, had a large mask bias, and could not be processed to the target pattern dimensions. Moreover, Comparative Example 3 not containing the repeating units represented by general formulas (1) to (4) had results inferior to the examples in all of storage stability, mask bias, and long-term reliability of the organic EL display device. [Explanation of symbols]
[0115] 1: Non-alkali glass substrate 2: First electrode (transparent electrode) 3: Auxiliary electrode 4: Insulating layer 5: Organic EL layer 6: Second electrode (non-transparent electrode)
Claims
1. A negative type photosensitive resin composition comprising: an alkali-soluble resin (A) containing a repeating unit represented by general formula (1) and / or general formula (2) and a repeating unit represented by general formula (3) and / or general formula (4); a radical polymerizable compound (B); a radical polymerization initiator (C); a coloring pigment (D); an organic solvent (E); and a resin (F) having a repeating unit represented by general formula (5) having a tertiary amino group in a side chain, a repeating unit having a carboxy group, and a repeating unit having an ethylenically unsaturated group. 【Chemistry 1】 【Chemistry 2】 【Chemistry 3】 【Chemistry 4】 【Chemistry 5】 (In general formula (1), R 1 represents a hydrogen atom or a methyl group, R 2 represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkylene ether group having 1 to 5 carbon atoms and 1 oxygen atom; R 3 represents an alkyl group, an alkoxy group, or an acyl group having 1 to 5 carbon atoms, l represents an integer of 0 to 4, and m represents an integer of 1 to 4. 3 When there are two or more R 3 may be different from each other or may be the same. In general formula (2), R 4 represents a hydrogen atom or a methyl group, R 5 represents an alkyl group, an alkoxy group, or an acyl group having 1 to 5 carbon atoms, n represents an integer of 0 to 4, and o represents an integer of 1 to 4. 5 When there are two or more R 5 may be different from each other or may be the same. In general formula (3), R 6 represents a hydrogen atom or a methyl group, R 7 represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkylene ether group having 1 to 5 carbon atoms and 1 oxygen atom. 8 represents an alkyl group having 1 to 5 carbon atoms, p represents an integer of 1 to 5, and q represents an integer of 0 to 5. 8 When there are two or more R 8 may be different from each other or may be the same. In general formula (4), R 9 represents a hydrogen atom or a methyl group, R 10 represents a single bond, an alkylene group having 1 to 5 carbon atoms, or an alkylene ether group having 1 to 5 carbon atoms and 1 oxygen atom. In general formula (5), R 11 represents a hydrogen atom or a methyl group, R 12 represents a single bond, an alkyl group having 1 to 5 carbon atoms, or an alkylene ether group having 1 to 5 carbon atoms and 1 oxygen atom, and R 13 and R 14 each independently represent an alkyl group having 1 to 5 carbon atoms, an alkoxy group, an alicyclic hydrocarbon group having 3 to 6 carbon atoms, or an aromatic hydrocarbon group having 6 to 10 carbon atoms.
2. 2. The negative type photosensitive resin composition according to claim 1, wherein a total molar ratio M1 of the repeating unit represented by general formula (1) and the repeating unit represented by general formula (2) relative to 100 mol% of all repeating units in the alkali-soluble resin (A) is 30 mol% or more and less than 70 mol%.
3. 3. The negative type photosensitive resin composition according to claim 1, wherein M1 / M2 is 0.4 to 1.5, where M1 is the total molar ratio of the repeating units represented by general formula (1) and the repeating units represented by general formula (2) and M2 is the total molar ratio of the repeating units represented by general formula (3) and the repeating units represented by general formula (4), relative to 100 mol% of all repeating units in the alkali-soluble resin (A).
4. 4. The negative type photosensitive resin composition according to claim 1, wherein the alkali-soluble resin (A) has a repeating unit represented by general formula (1).
5. R in the above general formula (1) 2 The negative type photosensitive resin composition according to any one of claims 1 to 4, wherein is a single bond.
6. A cured film obtained by curing the negative photosensitive resin composition according to any one of claims 1 to 5.
7. An organic electroluminescence display device comprising the cured film according to claim 6 .
Citation Information
Patent Citations
Photosensitive resin composition, cured film, color filter, and method for producing cured film
JP2018060136A
Negative-type photosensitive resin composition, cured film, element and display apparatus that include cured film, and production method for the same
JP2019023728A
Photosensitive composition for display element formation, hardened film and display element
JP2019046790A
Display element laminate and partition forming composition
JP2019179111A
Photosensitive resin composition, organic EL element partition wall, and organic EL element
JP6689434B1