Sulfide-based solid electrolytes
The Li a Ge 1+b Sb c P 2-b-c S 12 composition addresses the conductivity loss in Li10Ge1P2S12 by replacing P with Ge and Sb, achieving high ionic conductivity and water resistance in sulfide-based solid electrolytes.
Patent Information
- Application Number
- JP2022023370
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-02-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-02-18
AI Technical Summary
Li10Ge1P2S12 sulfide-based solid electrolytes experience a rapid decrease in ionic conductivity when part of the P is replaced with Sb, limiting water resistance improvement.
A composition of Li a Ge 1+b Sb c P 2-b-c S 12 is introduced, where 10≦a≦10.65, 0.35≦b≦0.65, and 0.075≦c≦0.15, allowing partial replacement of P with both Ge and Sb to maintain the LGPS structure and enhance ionic conductivity while improving water resistance.
The new composition achieves high ionic conductivity and high water resistance simultaneously, maintaining the LGPS structure with improved resistance to moisture.
Smart Images

Figure 0007574817000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a sulfide-based solid electrolyte. [Background technology]
[0002] In recent years, with the rapid spread of information-related devices and communication devices such as personal computers, video cameras, and mobile phones, the development of batteries to be used as power sources for these devices has become important. In the automobile industry, too, development of high-output, high-capacity batteries for electric vehicles or hybrid vehicles is underway.
[0003] In Non-Patent Document 1, Li 10 Ge1P2S 12 A sulfide-based solid electrolyte in which part of the P in the composition is replaced with Sb has been disclosed. [Prior art documents] [Non-patent literature]
[0004] [Non-Patent Document 1] Chem. Mater. 2020, 32, 2664-2672 Summary of the Invention [Problem to be solved by the invention]
[0005] Li 10 Ge1P2S 12 A sulfide-based solid electrolyte in which part of the P in the composition is replaced with Sb is expected to improve water resistance, but the ionic conductivity drops sharply by replacing P with Sb. In addition, since it is not possible to increase the amount of P replaced with Sb, water resistance is insufficient.
[0006] The present disclosure has been made in consideration of the above-mentioned circumstances, and has as its main object to provide a sulfide-based solid electrolyte having high ionic conductivity and high water resistance. [Means for solving the problem]
[0007] The sulfide-based solid electrolyte of the present disclosure has a composition of Li a Ge 1+b Sb c P 2-b-c S 12 A sulfide-based solid electrolyte represented by the formula: 10≦a≦10.65, 0.35≦b≦0.65, and 0.075≦c≦0.15.
[0008] In the sulfide-based solid electrolyte of the present disclosure, 0.35≦b≦0.5 may be satisfied. Effect of the Invention
[0009] The present disclosure can provide a sulfide-based solid electrolyte having high ionic conductivity and high water resistance. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a graph showing the results of ion conductivity versus the amount (mol) x of P in each of the sulfide-based solid electrolytes in Examples 1 to 4 and Comparative Examples 1 to 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] In this specification, the use of "to" indicating a numerical range means that the numerical values before and after it are included as the lower limit and upper limit. Furthermore, any combination of upper and lower limits in a numerical range can be used.
[0012] The sulfide-based solid electrolyte of the present disclosure has a composition of Li a Ge 1+b Sb c P 2-b-c S 12 A sulfide-based solid electrolyte represented by the formula: 10≦a≦10.65, 0.35≦b≦0.65, and 0.075≦c≦0.15.
[0013] The sulfide-based solid electrolyte of the present disclosure is Li a Ge 1+b Sb cP 2-b-c S 12 In the composition represented by the formula (1), a is 10≦a≦10.65, b is 0.35≦b≦0.65, and c is 0.075≦c≦0.15. In the sulfide-based solid electrolyte of the present disclosure, the amount of P substituted with Ge is 0.35 mol to 0.65 mol, and the amount of P substituted with Sb is 0.075 mol to 0.15 mol. In the sulfide-based solid electrolyte of the present disclosure, in the above composition, b may be 0.35≦b≦0.5. That is, in the sulfide-based solid electrolyte of the present disclosure, the amount of P substituted with Ge may be 0.35 mol to 0.5 mol. In the sulfide-based solid electrolyte of the present disclosure, in the above composition, Li may be 10 mol to 10.65 mol, P may be 1.275 mol to 1.575 mol, Ge may be 1.35 mol to 1.65 mol or 1.35 mol to 1.5 mol, and Sb may be 0.075 mol to 0.15 mol.
[0014] Standard composition is Li 10 GeP2S 12 In the LGPS-type solid electrolyte, when the P site is substituted with only Sb, the ionic conductivity decreases even with a small amount of substitution. In addition, the ionic radii of P and Sb are significantly different, so the amount of substitution at the P site is limited. According to the present disclosure, in an LGPS-type solid electrolyte, by replacing a portion of P with not only Sb but also Ge, it is possible to maintain the LPGS structure even in a composition with a small amount of P, and the ionic conductivity can be maintained. In addition, since the amount of P is less than that of conventional compositions, the water resistance can be improved, and it is possible to achieve both high ionic conductivity and high water resistance.
[0015] The sulfide-based solid electrolyte of the present disclosure may be used as a solid electrolyte in various batteries. The battery may be a primary battery or a secondary battery, but it may be a secondary battery in particular. The secondary battery can be repeatedly charged and discharged. The secondary battery is useful, for example, as a battery for vehicles. The battery may be an aqueous battery, a non-aqueous battery, an all-solid-state battery, or the like. The battery may be a lithium battery, a lithium ion battery, or the like. Furthermore, the all-solid-state battery may be an all-solid-state lithium secondary battery, an all-solid-state lithium ion secondary battery, or the like. The use of the battery is not particularly limited, but examples thereof include power sources for vehicles such as hybrid electric vehicles (HEVs), plug-in hybrid electric vehicles (PHEVs), electric vehicles (BEVs), gasoline-powered vehicles, and diesel-powered vehicles. In particular, the battery may be used as a driving power source for hybrid electric vehicles, plug-in hybrid electric vehicles, or electric vehicles. The battery of the present disclosure may also be used as a power source for moving objects other than vehicles (e.g., railways, ships, and aircraft), and may also be used as a power source for electrical appliances such as information processing devices. EXAMPLES
[0016] Example 1 [Li 10.35 Ge 1.35 Sb 0.075 P 1.575 S 12 Synthesis of Li2S (Furuuchi Chemical), GeS2 (Kojundo Chemical), Sb2S3 (Kojundo Chemical), S (Kojundo Chemical), and P2S5 (Aldrich) were weighed out to a molar ratio of 10.35:1.35:0.075:0.15:1.575, mixed in a mortar, and then placed in a 500ml ZrO2 pot. With a 5mmφ ZrO2 ball in the pot, the mixture was stirred at 300 rpm for 1 h for 20 cycles to obtain a precursor. This was then fired in a tubular furnace in an Ar flow atmosphere at a temperature above the crystallization temperature for 6 h to obtain a Ge, Sb substituted LGPS with the above composition.
[0017] Example 2 [Li 10.5 Ge 1.5 Sb 0.075 P 1.425 S 12 Synthesis of A Ge, Sb-substituted LGPS having the above composition was obtained in the same manner as in Example 1, except that the molar ratio at the time of weighing was Li2S:GeS2:Sb2S3:S:P2S5=10.5:1.5:0.075:0.15:1.425.
[0018] Example 3 [Li 10.5 Ge 1.5 Sb 0.15 P 1.35 S 12 Synthesis of A Ge, Sb-substituted LGPS having the above composition was obtained in the same manner as in Example 1, except that the molar ratio at the time of weighing was Li2S:GeS2:Sb2S3:S:P2S5=10.5:1.5:0.15:0.3:1.35.
[0019] Example 4 [Li 10.65 Ge 1.65 Sb 0.075 P 1.275 S 12 Synthesis of A Ge, Sb-substituted LGPS having the above composition was obtained in the same manner as in Example 1, except that the molar ratio at the time of weighing was Li2S:GeS2:Sb2S3:S:P2S5=10.65:1.65:0.075:0.15:1.275.
[0020] Comparative Example 1 [Li 10 Ge1P2S 12 Synthesis of LGPS having the above composition was obtained in the same manner as in Example 1, except that the molar ratio at the time of weighing was Li2S:GeS2:Sb2S3:S:P2S5=10:1:0:0:2.
[0021] Comparative Example 2 [Li 10 Ge1Sb 0.075 P 1.925 S 12 Synthesis of An Sb-substituted LGPS having the above composition was obtained in the same manner as in Example 1, except that the molar ratio at the time of weighing was Li2S:GeS2:Sb2S3:S:P2S5=10:1:0.075:0.15:1.925.
[0022] Comparative Example 3 [Li 10 Ge1Sb 0.15 P 1.85 S 12 Synthesis of An Sb-substituted LGPS having the above composition was obtained in the same manner as in Example 1, except that the molar ratio at the time of weighing was Li2S:GeS2:Sb2S3:S:P2S5=10:1:0.15:0.3:1.85.
[0023] Comparative Example 4 [Li 10 Ge1Sb 0.3 P 1.7 S 12 Synthesis of An Sb-substituted LGPS having the above composition was obtained in the same manner as in Example 1, except that the molar ratio at the time of weighing was Li2S:GeS2:Sb2S3:S:P2S5=10:1:0.3:0.6:1.7.
[0024] Comparative Example 5 [Li 10 Ge1Sb 0.5 P 1.5 S 12 Synthesis of An Sb-substituted LGPS having the above composition was obtained in the same manner as in Example 1, except that the molar ratio at the time of weighing was Li2S:GeS2:Sb2S3:S:P2S5=10:1:0.5:1:1.5.
[0025] Comparative Example 6 [Li 10.8 Ge 1.8 Sb 0.075 P 1.125 S 12 Synthesis of A Ge, Sb-substituted LGPS having the above composition was obtained in the same manner as in Example 1, except that the molar ratio at the time of weighing was Li2S:GeS2:Sb2S3:S:P2S5=10.8:1.8:0.075:0.15:1.125.
[0026] [Ionic conductivity measurement] The solid electrolytes of Examples 1 to 4 and Comparative Examples 1 to 6 were used to evaluate the ionic conductivity of the solid electrolyte under the following conditions. A powder cell was made by filling 100 mg of solid electrolyte into a cylinder and pressing it with a 6 ton pressure. Impedance measurements were performed in a thermostatic chamber at 25°C while the cell was placed in a desiccator. Ionic conductivity was calculated from the obtained resistance value and sample thickness. The results are shown in Figure 1. The ionic conductivity was 8.56 mS / cm in Example 1, 8.33 mS / cm in Example 2, 5.3 mS / cm in Example 3, 5.2 mS / cm in Example 4, 8.11 mS / cm in Comparative Example 1, 6.2 mS / cm in Comparative Example 2, 5.51 mS / cm in Comparative Example 3, 5.3 mS / cm in Comparative Example 4, 2.12 mS / cm in Comparative Example 5, and 1.87 mS / cm in Comparative Example 6.
[0027] [Evaluation Results] FIG. 1 is a graph showing the results of ion conductivity versus the amount (mol) x of P in each of the sulfide-based solid electrolytes in Examples 1 to 4 and Comparative Examples 1 to 6. 1, the results of Comparative Examples 1 to 5 show that when the amount of Sb substituted for P is 0.5 mol or more, the desired ionic conductivity cannot be obtained. The sulfide-based solid electrolytes of Examples 1 to 4 have higher ionic conductivity than the sulfide-based solid electrolytes of Comparative Examples 5 to 6, have high ionic conductivity of 5 mS / cm or more at room temperature of 25° C., and have higher water resistance than the sulfide-based solid electrolytes of Comparative Examples 1 to 4 because the amount of P in the composition is smaller than those of the sulfide-based solid electrolytes of Comparative Examples 1 to 4, and can achieve both high ionic conductivity and high water resistance.
Claims
1. The composition is Li a Ge 1+b Sb c P 2-b-c S 12 A sulfide-based solid electrolyte represented by the formula: A sulfide-based solid electrolyte, wherein 10≦a≦10.65, 0.35≦b≦0.65, and 0.075≦c≦0.
15.
2. The sulfide-based solid electrolyte according to claim 1, wherein 0.35≦b≦0.5.
Citation Information
Patent Citations
Amorphous-state sulfide solid electrolyte, preparation method thereof, and lithium ion battery
CN109301336A
Sulfide solid electrolyte, lithium cell, and method for manufacturing the sulfide solid electrolyte
JP2011129407A
Inorganic sulfide solid electrolyte with high atmospheric stability, its manufacturing method and its application
JP2022502341A