Impedance matching film for radio wave absorber, film with impedance matching film for radio wave absorber, radio wave absorber, and laminate for radio wave absorber

The impedance matching film with controlled thickness and composition stabilizes sheet resistance, ensuring effective radio wave absorption at high temperatures.

JP7575197B2Active Publication Date: 2024-10-29NITTO DENKO CORP
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020059170
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-03-29
Filing Date
2020-03-27
Publication Date
2024-10-29
Estimated Expiration
2040-03-27

AI Technical Summary

Technical Problem

Existing radio wave absorber technologies fail to maintain impedance matching at high temperatures due to significant changes in sheet resistance.

Method used

An impedance matching film with specific thickness (10-200 nm) and sheet resistance (200Ω/□ or more) containing metallic and non-metallic elements, with limited oxygen content, is used to stabilize resistance values under high temperatures.

Benefits of technology

The film effectively maintains desired sheet resistance and radio wave absorption performance even in high-temperature environments, reducing changes in impedance matching.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575197000003
    Figure 0007575197000003
  • Figure 0007575197000004
    Figure 0007575197000004
  • Figure 0007575197000005
    Figure 0007575197000005
Patent Text Reader

Abstract

To provide a novel impedance-matching film for an electromagnetic wave absorber, which is advantageous in suppressing the change in sheet resistance when exposed to a high-temperature environment from the viewpoint of impedance matching.SOLUTION: An impedance-matching film 10 comprises a metal element and a nonmetallic element. The impedance-matching film 10 has a thickness of 10-200 nm. The impedance-matching film 10 has a sheet resistance of 200 Ω / sq. or larger. In the impedance-matching film 10, the atomic number based content of oxygen atoms is less than 50%.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an impedance matching film for a radio wave absorber, an impedance matching film-attached film for a radio wave absorber, a radio wave absorber, and a laminate for a radio wave absorber. [Background technology]

[0002] A technique for achieving impedance matching by using an alloy in a resistive film for a radio wave absorber to match the impedance of the surface of the radio wave absorber to the characteristic impedance of air is conventionally known.

[0003] For example, Patent Document 1 proposes a resistive film for a λ / 4 type radio wave absorber made of an alloy containing 5% by weight or more of molybdenum. In this resistive film for a λ / 4 type radio wave absorber, the surface resistance is adjusted to a predetermined range at a film thickness of 5 to 6 nm by adjusting the nickel content and chromium content of the alloy. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2018-56562 A Summary of the Invention [Problem to be solved by the invention]

[0005] In Patent Document 1, the change over time in the surface resistance value of the resistive film at 25° C. is measured. However, Patent Document 1 does not evaluate the change over time in the surface resistance value of the resistive film when exposed to a high-temperature environment (e.g., an environment of 80° C.).

[0006] In consideration of these circumstances, the present invention provides a novel impedance matching film for a radio wave absorber, which is advantageous in suppressing a change in sheet resistance when exposed to a high-temperature environment from the viewpoint of impedance matching. [Means for solving the problem]

[0007] The present invention relates to Contains a metal element and a non-metal element, The thickness is 10 to 200 nm. It has a sheet resistance of 200Ω / □ or more. The content of oxygen atoms based on the atomic number is less than 50%. An impedance matching film for an electromagnetic wave absorber is provided.

[0008] The present invention also provides a method for producing a semiconductor device comprising the steps of: A substrate; The impedance matching film for a radio wave absorber according to the present invention is provided. We provide a film with impedance matching membrane for use as a radio wave absorber.

[0009] The present invention also provides a method for producing a semiconductor device comprising the steps of: The impedance matching film for a radio wave absorber, A conductor that reflects radio waves; a dielectric layer disposed between the impedance matching film for the radio wave absorber and the conductor in a thickness direction of the impedance matching film for the radio wave absorber; Provide a radio wave absorber.

[0010] The present invention also provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: The impedance matching film for a radio wave absorber, A dielectric layer is disposed in contact with the impedance matching film for the radio wave absorber in a thickness direction of the impedance matching film for the radio wave absorber. A laminate for a radio wave absorber is provided. Effect of the Invention

[0011] The impedance matching film for a radio wave absorber described above is advantageous in suppressing changes in sheet resistance from the viewpoint of impedance matching when exposed to a high-temperature environment. [Brief description of the drawings]

[0012] [Figure 1]FIG. 1 is a cross-sectional view showing an example of an impedance matching film for a radio wave absorber according to the present invention. [Figure 2A] FIG. 2A is a cross-sectional view showing an example of a radio wave absorber according to the present invention. [Figure 2B] FIG. 2B is a cross-sectional view showing a modification of the radio wave absorber shown in FIG. 2A. [Figure 2C] FIG. 2C is a cross-sectional view showing another modified example of the radio wave absorber shown in FIG. 2A. [Diagram 3] FIG. 3 is a cross-sectional view showing another example of a radio wave absorber according to the present invention. [Figure 4A] FIG. 4A is a cross-sectional view showing still another example of a radio wave absorber according to the present invention. [Figure 4B] FIG. 4B is a cross-sectional view showing one example of the laminate for a radio wave absorber according to the present invention. [Figure 5A] FIG. 5A is a cross-sectional view showing still another example of a radio wave absorber according to the present invention. [Figure 5B] FIG. 5B is a cross-sectional view showing another example of the laminate for a radio wave absorber according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described with reference to the accompanying drawings. It should be noted that the present invention is not limited to the following embodiments.

[0014] 1, the impedance matching film 10 for a radio wave absorber is provided by, for example, an impedance matching film-attached film 15 for a radio wave absorber. The impedance matching film 10 for a radio wave absorber is a resistive film. The impedance matching film-attached film 15 for a radio wave absorber includes a substrate 22 and the impedance matching film 10 for a radio wave absorber. The impedance matching film 10 for a radio wave absorber is formed on, for example, one of the main surfaces of the substrate 22.

[0015] The impedance matching film 10 includes a metal element and a nonmetal element. In addition, the impedance matching film 10 has a thickness of 10 to 200 nm and a sheet resistance of 200 Ω / □ or more. Furthermore, the impedance matching film 10 has an oxygen atom content of less than 50% based on the atomic number. Therefore, an indium tin oxide (ITO) film is not included in the impedance matching film 10. In this specification, semimetal elements such as silicon, germanium, arsenic, antimony, and tellurium are treated as nonmetal elements. The impedance matching film 10 is, for example, a resistive film adjusted so that the impedance seen from the front surface is equal to the characteristic impedance of a plane wave.

[0016] The impedance matching film 10 has a thickness of 10 to 200 nm, and therefore, when exposed to a high-temperature environment (e.g., 80°C), it is easy to maintain a desired sheet resistance from the viewpoint of impedance matching. This is because, even if the vicinity of the surface of the impedance matching film is altered in a high-temperature environment, the volume occupied by the altered portion in the impedance matching film 10 is small. On the other hand, the resistive film for a λ / 4 type radio wave absorber described in Patent Document 1 has a film thickness of, for example, 5 to 6 nm. Since this resistive film is thin, when the vicinity of the surface of the resistive film is altered in a high-temperature environment, the volume occupied by the altered portion in the resistive film is large, and the influence on the characteristics of the resistive film for impedance matching is large. For this reason, it is difficult to say that the technology described in Patent Document 1 is advantageous for suppressing the change in the sheet resistance of the resistive film from the viewpoint of impedance matching when exposed to a high-temperature environment.

[0017] The thickness of the impedance matching film 10 may be 11 nm or more, 13 nm or more, or 15 nm or more.

[0018] The thickness of the impedance matching film 10 is 200 nm or less. This makes it possible to suppress warping of the impedance matching film 10, and makes it difficult for cracks to occur in the impedance matching film 10. The thickness of the impedance matching film 10 may be 180 nm or less, 160 nm or less, or 150 nm or less.

[0019] Since the impedance matching film 10 has a sheet resistance of 200 Ω / □ or more, the radio wave absorber provided using the impedance matching film 10 can easily exhibit the desired radio wave absorbing performance.

[0020] The sheet resistance of the impedance matching film 10 may be 220 Ω / □ or more, 250 Ω / □ or more, or 280 Ω / □ or more.

[0021] The upper limit of the sheet resistance of the impedance matching film 10 is not limited to a specific value. The sheet resistance of the impedance matching film 10 may vary depending on the characteristics of other components of the radio wave absorber. In one example of the radio wave absorber, the sheet resistance of the impedance matching film 10 is, for example, 600Ω / □ or less. The sheet resistance of the impedance matching film 10 may be 580Ω / □ or less, 550Ω / □ or less, or 520Ω / □ or less. For example, when the radio wave absorber does not contain a loss material such as a dielectric loss material or a magnetic loss material, the upper limit of the sheet resistance of the impedance matching film 10 may be adjusted to such a range. In another example of the radio wave absorber, the sheet resistance of the impedance matching film 10 is, for example, 10MΩ (megohms) / □ or less, 8MΩ / □ or less, 5MΩ / □ or less, or 3MΩ / □ or less. For example, when the radio wave absorber contains a loss material such as a dielectric loss material or a magnetic loss material, the upper limit of the sheet resistance of the impedance matching film 10 may be adjusted to such a range.

[0022] The impedance matching film 10 is, for example, 0.40×10 -3 It has a resistivity of Ω·cm or more. This makes it easy for the impedance matching film 10 to have a desired sheet resistance from the standpoint of impedance matching while having a thickness of 10 to 200 nm.

[0023] The resistivity of the impedance matching film 10 is 0.44×10 -3 It may be 0.50×10 Ω cm or more. -3 It may be 0.56×10 Ω cm or more. -3It may be Ω·cm or more.

[0024] The upper limit of the resistivity of the impedance matching film 10 is not limited to a specific value. The resistivity of the impedance matching film 10 may vary depending on the characteristics of other components of the radio wave absorber. In one example of the radio wave absorber, the resistivity of the impedance matching film 10 is, for example, 8.0×10 -3 The resistivity of the impedance matching film 10 is 7.7×10 -3 It may be less than 7.3×10 Ω cm. -3 It may be less than 7×10 Ω cm. -3 Ω·cm or less. For example, when the radio wave absorber does not contain a loss material such as a dielectric loss material or a magnetic loss material, the upper limit of the sheet resistance of the impedance matching film 10 can be adjusted to such a range. In another example of the radio wave absorber, the resistivity of the impedance matching film 10 is, for example, 150 Ω·cm or less, and may be 100 Ω·cm or less, 80 Ω·cm or less, or 50 Ω·cm or less. For example, when the radio wave absorber contains a loss material such as a dielectric loss material or a magnetic loss material, the upper limit of the sheet resistance of the impedance matching film 10 can be adjusted to such a range.

[0025] In the impedance matching film 10, the sheet resistance change rate Cs determined by the following formula (1) is, for example, 30% or less. In formula (1), Ri [Ω / □] is the initial sheet resistance of the impedance matching film 10, and Rt [Ω / □] is the sheet resistance of the impedance matching film 10 after the environmental temperature of the impedance matching film 10 is kept at 80°C for 24 hours. If the sheet resistance change rate Cs of the impedance matching film 10 is 30% or less, the radio wave absorption performance is likely to be maintained even if the radio wave absorber is exposed to a high-temperature environment. It is most desirable that the sheet resistance change rate Cs is 0%. Cs[%]=100×|Rt-Ri| / Ri Formula (1)

[0026] The sheet resistance change rate Cs of the impedance matching film 10 may be 28% or less, 25% or less, or 23% or less.

[0027] The nonmetallic element contained in the impedance matching film 10 is not limited to a specific element, so long as the impedance matching film 10 has a thickness of 10 to 200 nm and a sheet resistance of 200 Ω / □ or more. The nonmetallic element contained in the impedance matching film 10 is, for example, at least one element selected from the group consisting of B, C, N, O, F, Si, S, and Ge. In this case, the impedance matching film 10 is more likely to maintain a desired sheet resistance from the viewpoint of impedance matching when exposed to a high-temperature environment.

[0028] The metal element contained in the impedance matching film 10 is not limited to a specific element, so long as the impedance matching film 10 has a thickness of 10 to 200 nm and a sheet resistance of 200 Ω / □ or more. The metal element contained in the impedance matching film 10 is, for example, at least one element selected from the group consisting of Ni, Cr, Ti, W, Mo, Cu, Al, Sn, Pd, Ta, Rh, Au, Mg, Fe, Mn, Co, and V. In this case, the impedance matching film 10 is more likely to maintain a desired sheet resistance from the viewpoint of impedance matching when exposed to a high-temperature environment.

[0029] The metal element contained in the impedance matching film 10 may be at least one element selected from the group consisting of Ni, Cr, Mo, and Ti. In this case, the impedance matching film 10 can more reliably maintain a desired sheet resistance from the viewpoint of impedance matching when exposed to a high-temperature environment.

[0030] The atomic number-based content of the metal elements contained in the impedance matching film 10 is not limited to a specific value. The content exceeds 0%, and may be 5% or more, 10% or more, 15% or more, or 20% or more. The atomic number-based content of the metal elements contained in the impedance matching film 10 is, for example, 90% or less, 85% or less, 80% or less, 75% or less, or 70% or less.

[0031] When the metal elements contained in the impedance matching film 10 include at least one element selected from the group consisting of Ni, Cr, Mo, and Ti, the total content of Ni, Cr, Mo, and Ti based on the atomic number is, for example, 10% or more. In this case, the impedance matching film 10 is more likely to maintain a desired sheet resistance from the viewpoint of impedance matching when exposed to a high-temperature environment.

[0032] In the impedance matching film 10, the total content of Ni, Cr, Mo, and Ti based on the atomic number may be 11% or more, 13% or more, or 15% or more. In the impedance matching film 10, the total content of Ni, Cr, Mo, and Ti based on the atomic number may be, for example, 90% or less, 85% or less, 80% or less, 75% or less, or 70% or less.

[0033] The substrate 22 serves as, for example, a support for supporting the impedance matching film 10. The impedance matching film 10 is formed on one main surface of the substrate 22 by, for example, sputtering using a predetermined target material. In this case, for example, a predetermined target material containing a metal element and a nonmetal element is used. In addition to the composition of the target material, by adjusting predetermined conditions such as the ratio of the volume flow rate of an active gas such as oxygen gas to the volume flow rate of a gas supplied around the substrate 22 in sputtering, the impedance matching film 10 can be formed so that the content of oxygen atoms based on the atomic number is less than 50%. In some cases, the impedance matching film 10 may be formed using a method such as ion plating or coating (e.g., bar coating).

[0034] As shown in Fig. 2A, a radio wave absorber 1a can be provided by using an impedance matching film 10. The radio wave absorber 1a includes the impedance matching film 10, a conductor 30, and a dielectric layer 20. The conductor 30 reflects radio waves. The dielectric layer 20 is disposed between the impedance matching film 10 and the conductor 30 in the thickness direction of the impedance matching film 10.

[0035] The wave absorber 1a is, for example, a λ / 4 type wave absorber. O The radio wave absorber 1a is designed so that when a radio wave of this type is incident, the radio wave reflected by the surface of the impedance matching film 10 (surface reflection) interferes with the radio wave reflected by the conductor 30 (rear reflection). In a λ / 4 type radio wave absorber, as shown in the following formula (2), the thickness t of the dielectric layer and the relative dielectric constant ε of the dielectric layer r The wavelength of the radio wave to be absorbed is λ O That is, by appropriately adjusting the relative dielectric constant and thickness of the dielectric layer, it is possible to set the wavelength of the radio waves to be absorbed. r ) is the relative dielectric constant ε r means the square root of λ O =4t×sqrt(ε r ) Formula (2)

[0036] Since the radio wave absorber 1a is provided with the impedance matching film 10, the radio wave absorber 1a is likely to maintain the desired radio wave absorbing performance even when exposed to a high-temperature environment.

[0037] In designing a radio wave absorber, for example, the sheet resistance of the impedance matching film 10 is determined using transmission theory so that the impedance seen from the front side of the impedance matching film 10 is equal to the characteristic impedance of a plane wave. In a radio wave absorber, the sheet resistance required for the impedance matching film 10 can vary depending on the expected incident angle of the radio wave incident on the radio wave absorber.

[0038] The conductor 30 has a predetermined conductivity, but is not particularly limited as long as it can reflect the radio waves to be absorbed. As shown in Fig. 2A, the conductor 30 is formed, for example, in a layered shape. In this case, the conductor 30 has a sheet resistance lower than the sheet resistance of the impedance matching film 10. The conductor 30 may have a shape other than a layered shape.

[0039] The conductor 30 contains, for example, indium tin oxide, which tends to make the conductor 30 highly transparent.

[0040] The content of tin oxide in the indium tin oxide of the conductor 30 is, for example, 5 to 15 mass %. In this case, the conductor 30 can be formed of indium tin oxide in a stable polycrystalline state by annealing treatment. As a result, the wave absorber 1a is more likely to exhibit the desired wave absorbing performance more reliably when exposed to a high-temperature environment for a long period of time.

[0041] The conductor 30 may contain at least one selected from the group consisting of aluminum, copper, iron, an aluminum alloy, a copper alloy, and an iron alloy. In this case, it is easy to achieve the desired conductivity while reducing the thickness of the conductor 30.

[0042] The thickness of the conductor 30 is not limited to a specific thickness. For example, when the conductor 30 is made of indium tin oxide, the conductor 30 has a thickness of, for example, 20 to 200 nm, and preferably a thickness of 50 to 150 nm. This allows the wave absorber 1a to exhibit the desired wave absorbing performance, and makes the conductor 30 less susceptible to cracking.

[0043] When the conductor 30 is at least one selected from the group consisting of aluminum, copper, iron, an aluminum alloy, a copper alloy, and an iron alloy, the conductor 30 has a thickness of, for example, 30 nm to 100 μm, and preferably has a thickness of 50 nm to 50 μm.

[0044] The dielectric layer 20 has a relative dielectric constant of, for example, 2.0 to 20.0. In this case, it is easy to adjust the thickness of the dielectric layer 20, and therefore easy to adjust the radio wave absorbing performance of the radio wave absorber 1a. The relative dielectric constant of the dielectric layer 20 is, for example, the relative dielectric constant at 10 GHz measured according to a cavity resonance method.

[0045] The dielectric layer 20 is formed of, for example, a predetermined polymer. The dielectric layer 20 contains, for example, at least one polymer selected from the group consisting of ethylene-vinyl acetate copolymer, vinyl chloride resin, urethane resin, acrylic resin, acrylic urethane resin, polyethylene, polypropylene, silicone, polyethylene terephthalate, polyethylene naphthalate, polycarbonate, polyimide, and cycloolefin polymer. In this case, the thickness of the dielectric layer 20 is easy to adjust, and the manufacturing cost of the radio wave absorber 1a can be kept low. The dielectric layer 20 can be produced, for example, by heat pressing a predetermined resin composition.

[0046] The dielectric layer 20 may be formed as a single layer, or may be formed of multiple layers made of the same or different materials. When the dielectric layer 20 has n layers (n is an integer of 2 or more), the relative dielectric constant of the dielectric layer 20 is determined, for example, as follows. The relative dielectric constant ε of each layer is i (i is an integer from 1 to n). Next, the measured relative dielectric constant ε i The thickness of the layer t i multiplied by the ratio of the thickness of the dielectric layer 20 to the total thickness T to obtain ε i ×(t i / T) for all layers. i ×(t i / T) to determine the relative dielectric constant of the dielectric layer 20.

[0047] 2A, the dielectric layer 20 includes, for example, a first layer 21, a second layer 22, and a third layer 23. The first layer 21 is disposed between the second layer 22 and the third layer 23. The first layer 21 includes, for example, at least one polymer selected from the group consisting of ethylene-vinyl acetate copolymer, vinyl chloride resin, urethane resin, acrylic resin, acrylic urethane resin, polyethylene, polypropylene, silicone, polyethylene terephthalate, polyethylene naphthalate, polycarbonate, polyimide, and cycloolefin polymer.

[0048] In the radio wave absorber 1a, the second layer 22 also serves as a base material for the impedance matching film 10. The second layer 22 is disposed, for example, closer to the conductor 30 than the impedance matching film 10. As shown in FIG. 2B, the second layer 22 may be disposed farther from the conductor 30 than the impedance matching film 10. In this case, the first layer 21 and the third layer 23 form the dielectric layer 20. In this case, the impedance matching film 10 and the dielectric layer 20 are protected by the second layer 22, and the radio wave absorber 1a has high durability. In this case, for example, the impedance matching film 10 may be in contact with the first layer 21. The second layer 22 also serves as an auxiliary material for adjusting the thickness of the impedance matching film 10 with high precision. The material of the second layer 22 is, for example, polyethylene terephthalate (PET), polyethylene naphthalate (PEN), acrylic resin (PMMA), polycarbonate (PC), polyimide (PI), or cycloolefin polymer (COP). Among these, from the viewpoint of a balance between good heat resistance, dimensional stability, and manufacturing costs, the material of the second layer 22 is preferably PET.

[0049] The substrate 22 has a thickness of, for example, 10 to 150 μm, and preferably 15 to 100 μm, so that the bending rigidity of the substrate 22 is low and the occurrence of wrinkles or deformation in the substrate 22 can be suppressed when the impedance matching film 10 is formed.

[0050] In the radio wave absorber 1a, the third layer 23 supports, for example, a layered conductor 30. In this case, the layered conductor 30 is, for example, a metal foil or an alloy foil. The layered conductor 30 may be formed by forming a film on the third layer 23 using a method such as sputtering, ion plating, or coating (for example, bar coating). For example, in the radio wave absorber 1a, the third layer 23 is disposed at a position closer to the impedance matching film 10 than the layered conductor 30, and constitutes a part of the dielectric layer 20. Note that, as shown in FIG. 2C, the third layer 23 may be disposed at a position farther from the impedance matching film 10 than the layered conductor 30. In this case, for example, the layered conductor 30 is in contact with the first layer 21.

[0051] As the material of the third layer 23, for example, the materials exemplified as the materials of the second layer 22 can be used. The material of the third layer 23 may be the same as or different from the material of the second layer 22. From the viewpoint of a balance between good heat resistance, dimensional stability, and manufacturing costs, the material of the third layer 23 is desirably PET.

[0052] The third layer 23 has a thickness of, for example, 10 to 150 μm, and preferably 15 to 100 μm. This allows the bending rigidity of the third layer 23 to be low, and can suppress the occurrence of wrinkles or deformation in the third layer 23 when forming the layered conductor 30. The third layer 23 may be omitted in some cases.

[0053] The first layer 21 may be composed of multiple layers, particularly when the first layer 21 is in contact with at least one of the impedance matching film 10 and the layered conductor 30 as shown in FIG. 2B or 2C.

[0054] The first layer 21 may or may not have adhesiveness. When the first layer 21 has adhesiveness, an adhesive layer may be arranged in contact with at least one of the two main surfaces of the first layer 21, or an adhesive layer may not be arranged in contact with both main surfaces. When the first layer 21 does not have adhesiveness, an adhesive layer is desirably arranged in contact with both main surfaces of the first layer 21. When the dielectric layer 20 includes the second layer 22, even if the second layer 22 does not have adhesiveness, an adhesive layer may not be arranged in contact with both main surfaces of the second layer 22. In this case, an adhesive layer may be arranged in contact with one main surface of the second layer 22. When the dielectric layer 20 includes the third layer 23, even if the third layer 23 does not have adhesiveness, an adhesive layer may not be arranged in contact with both main surfaces of the third layer 23. An adhesive layer may be arranged in contact with at least one main surface of the third layer 23.

[0055] The radio wave absorber 1a is designed to absorb radio waves of a desired wavelength. The type of radio waves that the radio wave absorber 1a can absorb is not particularly limited. The radio waves that the radio wave absorber 1a can absorb may be, for example, millimeter waves or submillimeter waves in a specific frequency band.

[0056] The wave absorber 1a may contain at least one of a dielectric loss material and a magnetic loss material. In other words, the wave absorber 1a may be a dielectric loss type wave absorber or a magnetic loss type wave absorber. In this case, the sheet resistance required for the impedance matching film 10 tends to be high. The dielectric layer 20 may contain at least one of a dielectric loss material and a magnetic loss material. Also, the material forming the impedance matching film 10 may be a magnetic material.

[0057] The radio wave absorber 1a can be modified from various viewpoints. For example, the radio wave absorber 1a may be modified to the radio wave absorber 1b shown in FIG. 3, the radio wave absorber 1c shown in FIG. 4A, or the radio wave absorber 1d shown in FIG. 5A. The radio wave absorbers 1b, 1c, and 1d are configured similarly to the radio wave absorber 1a, except for the parts that are particularly described. The components of the radio wave absorbers 1b, 1c, and 1d that are the same as or correspond to the components of the radio wave absorber 1a are denoted by the same reference numerals, and detailed description thereof will be omitted. The description of the radio wave absorber 1a also applies to the radio wave absorbers 1b, 1c, and 1d, so long as there is no technical contradiction.

[0058] 3, the radio wave absorber 1b further includes an adhesive layer 40a. In the radio wave absorber 1b, the conductor 30 is disposed between the dielectric layer 20 and the adhesive layer 40a.

[0059] For example, the radio wave absorber 1b can be attached to a given article by bringing the adhesive layer 40a into contact with the article and pressing the radio wave absorber 1b against the article, thereby obtaining an article with a radio wave absorber.

[0060] The adhesive layer 40a contains, for example, a rubber-based adhesive, an acrylic-based adhesive, a silicone-based adhesive, or a urethane-based adhesive. The radio wave absorber 1b may further include a separator (not shown). In this case, the separator covers the adhesive layer 40a. The separator is typically a film that can maintain the adhesive force of the adhesive layer 40a when covering the adhesive layer 40a and can be easily peeled off from the adhesive layer 40a. The separator is, for example, a film made of a polyester resin such as PET. By peeling off the separator, the adhesive layer 40a is exposed, and the radio wave absorber 1b can be attached to an article.

[0061] In the radio wave absorber, the dielectric layer 20 may have adhesiveness to the conductor 30. For example, as shown in FIG. 4A, in a radio wave absorber 1c, the dielectric layer 20 has a plurality of layers including an adhesive layer 40b. The adhesive layer 40b is in contact with the conductor 30. The adhesive layer 40b contains, for example, a rubber-based adhesive, an acrylic-based adhesive, a silicone-based adhesive, or a urethane-based adhesive. The adhesive layer 40b is disposed, for example, between the first layer 21 and the conductor 30.

[0062] 4A, the dielectric layer 20 further includes an adhesive layer 40c. The adhesive layer 40c is in contact with, for example, the second layer 22. The radio wave absorber 1c may be modified so that the adhesive layer 40c is in contact with the impedance matching film 10. The adhesive layer 40c includes, for example, a rubber-based adhesive, an acrylic-based adhesive, a silicone-based adhesive, or a urethane-based adhesive. The adhesive layer 40c is disposed, for example, between the first layer 21 and the second layer 22.

[0063] The wave absorber 1c can be produced, for example, by using a laminate 50a for a wave absorber as shown in Fig. 4B. The laminate 50a for a wave absorber includes an impedance matching film 10 and a dielectric layer 20. The dielectric layer 20 is disposed in contact with the impedance matching film 10 in the thickness direction of the impedance matching film 10.

[0064] According to the laminate 50a for a radio wave absorber, the dielectric layer 20 has adhesiveness, for example, on the main surface remote from the impedance matching film 10. In this case, for example, by bringing the dielectric layer 20 into contact with the conductor 30 and pressing the laminate 50a for a radio wave absorber against the conductor 30, the laminate 50a for a radio wave absorber is attached to the conductor 30, and the radio wave absorber 1c can be produced.

[0065] 4B, in the wave absorber laminate 50a, the dielectric layer 20 has, for example, a plurality of layers including an adhesive layer 40b. The adhesive layer 40b is disposed farthest from the impedance matching film 10 among the plurality of layers constituting the dielectric layer 20.

[0066] The laminate 50a for a radio wave absorber may further include a separator (not shown). In this case, the separator covers the adhesive layer 40b. The separator is typically a film that can maintain the adhesive force of the adhesive layer 40b when covering the adhesive layer 40b and can be easily peeled off from the adhesive layer 40b. The separator is, for example, a film made of a polyester resin such as PET. By peeling off the separator, the adhesive layer 40b is exposed, and the laminate 50a for a radio wave absorber can be attached to the conductor 30.

[0067] 5A, in a radio wave absorber 1d, the first layer 21 is in contact with the conductor 30. The first layer 21 has, for example, adhesive properties to the conductor 30. The first layer 21 is in contact with, for example, the second layer 22. The first layer 21 has, for example, adhesive properties to the second layer 22. The radio wave absorber 1d may be modified so that the first layer 21 is in contact with the impedance matching film 10. In this case, the first layer 21 has, for example, adhesive properties to the impedance matching film 10.

[0068] The wave absorber 1d can be produced, for example, by using a laminate 50b for a wave absorber as shown in Fig. 5B. The laminate 50b for a wave absorber includes an impedance matching film 10 and a dielectric layer 20. The dielectric layer 20 is disposed in contact with the impedance matching film 10 in the thickness direction of the impedance matching film 10.

[0069] In the laminate 50b for a radio wave absorber, the dielectric layer 20 has adhesiveness on the main surface remote from the impedance matching film 10. For example, the first layer 21 has adhesiveness. For example, by bringing the first layer 21 into contact with the conductor 30 and pressing the laminate 50b for a radio wave absorber against the conductor 30, the laminate 50b for a radio wave absorber is attached to the conductor 30, and the radio wave absorber 1d can be produced.

[0070] The laminate 50b for a radio wave absorber may further include a separator (not shown). In this case, the separator covers the surface of the dielectric layer 20 that is to come into contact with the conductor 30. The separator is typically a film that can maintain the adhesive force of the surface of the dielectric layer 20 that is to come into contact with the conductor 30 when covering the surface of the dielectric layer 20 that is to come into contact with the conductor 30 and can be easily peeled off from the dielectric layer 20. The separator is, for example, a film made of a polyester resin such as PET. By peeling off the separator, the surface of the dielectric layer 20 that is to come into contact with the conductor 30 is exposed, and the laminate 50b for a radio wave absorber can be attached to the conductor 30.

[0071] The laminate for a radio wave absorber is not limited to a specific configuration, so long as it comprises an impedance matching film 10 and a dielectric layer 20, and the dielectric layer 20 is arranged in contact with the impedance matching film 10 in the thickness direction of the impedance matching film 10. EXAMPLES

[0072] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples. First, the evaluation methods for the examples and comparative examples will be described.

[0073] [X-ray diffraction] The thickness of the impedance matching film of the impedance matching film-attached film according to each of the examples and comparative examples was measured by an X-ray reflectance method using an X-ray diffraction device (manufactured by Rigaku Corporation, product name: RINT2200). The results are shown in Table 1.

[0074] [TEM-EDX] Using a focused ion beam (FIB) processing and observation device (manufactured by Hitachi High-Technologies Corporation, FB-2200), samples for TEM-EDX were prepared from the impedance matching films according to the examples and comparative examples by FIB microsampling. The thickness of the sample was 80 nm. Using a TEM-EDX device, EDX was performed on a specific region of the cross section of the sample to examine the content of each element based on the atomic number. The results are shown in Table 1. The TEM-EDX device was configured by combining a TEM (manufactured by JEOL Ltd., product name: JEM-2800) and an EDX device (manufactured by Thermo Fisher Scientific, product name: NORAN System 7). The region where EDX was performed was a region having a length of 400 nm in a direction perpendicular to the thickness direction at the center position in the thickness direction of the impedance matching film.

[0075] [Resistivity] Using a non-contact resistance measuring device (manufactured by Napson, product name: NC-80MAP), the initial sheet resistance Ri [Ω / □] of the impedance matching film according to each example and comparative example was measured by eddy current measurement method in accordance with JIS Z 2316. In each example and comparative example, the resistivity was determined by calculating the product of the thickness of the impedance matching film measured as described above and the initial sheet resistance Ri [Ω / □] of the impedance matching film measured as described above. The results are shown in Table 1.

[0076] [Heating test] The impedance matching film-attached films of each Example and Comparative Example were exposed to an environment of 80°C for 24 hours. After that, the sheet resistance Rt [Ω / □] of the impedance matching films of each Example and Comparative Example after the heating test was measured by an eddy current measurement method in accordance with JIS Z 2316 using a non-contact resistance measuring device (manufactured by Napson, product name: NC-80MAP). From this measurement result and the initial sheet resistance Ri [Ω / □] of the impedance matching film measured as described above, the sheet resistance change rate Cs of the impedance matching film of each Example was calculated based on the above formula (1). The results are shown in Table 1.

[0077] [Radio wave absorption performance] With reference to JIS R 1679:2007, radio waves of frequencies between 60 and 90 GHz were incident at an incident angle of 0° on the samples of each of the examples and comparative examples fixed to a sample holder, and the return loss at each frequency was determined using an Anritsu vector network analyzer. The return loss is the absolute value |S| of the value calculated according to the following formula (3). In formula (3), P0 is the power of the transmitted radio waves when the radio waves are incident on the measurement target at a predetermined incident angle, and P i is the power of the received radio wave in that case. Instead of the samples according to each embodiment and each comparative example, an aluminum plate was fixed to a sample holder, and the return loss |S| when radio waves were vertically incident on this plate was considered to be 0 dB, and this was used as the reference for the return loss |S| of each sample. This plate had a surface dimension of 30 cm square and a thickness of 5 mm. The maximum value of return loss |S| and the frequency showing this maximum value (peak absorption frequency) were determined for each sample. The results are shown in Table 2. If the maximum value of return loss |S| is 10 dB or more, it can be evaluated as having good radio wave absorption performance. S[dB]=10×log|P i / P0| Expression (3)

[0078] <Example 1> On a PET film having a thickness of 23 μm, a target material containing Cr (chromium), Ti (titanium), and O (oxygen) was used, and sputtering was performed while supplying argon gas to the periphery of the PET film, to form an impedance matching film according to Example 1. In this manner, a film with an impedance matching film according to Example 1 was obtained.

[0079] An acrylic resin having a relative dielectric constant of 2.6 was molded to a thickness of 560 μm to obtain an acrylic resin layer. The impedance matching film-attached film according to Example 1 was laminated on the acrylic resin layer so that the impedance matching film of the impedance matching film-attached film according to Example 1 was in contact with the acrylic resin layer. Next, a film with a reflector was obtained in which a PET layer was formed on both sides of an Al (aluminum) film having a thickness of 7 μm. In this film with a reflector, the PET layer formed on one main surface of the aluminum film had a thickness of 25 μm, and the PET layer formed on the other main surface of the aluminum film had a thickness of 9 μm. The film with a reflector was laminated on the acrylic resin layer so that the PET layer having a thickness of 25 μm in the film with a reflector was in contact with the acrylic resin layer. In this manner, a sample according to Example 1 was obtained.

[0080] <Example 2> On a PET film having a thickness of 23 μm, a target material made of Cr (chromium) was used to perform sputtering while supplying argon gas and nitrogen gas to the periphery of the PET film, forming an impedance matching film according to Example 2. In this manner, a film with an impedance matching film according to Example 2 was obtained. It is believed that oxygen was detected in the impedance matching film according to Example 2 due to the influence of a small amount of residual oxygen that was taken into the chamber during sputtering.

[0081] A sample according to Example 2 was produced in the same manner as in Example 1, except that the impedance matching film according to Example 2 was used instead of the impedance matching film according to Example 1.

[0082] <Example 3> On a PET film having a thickness of 23 μm, sputtering was performed using a target material made of Hastelloy C-276 while supplying argon gas and nitrogen gas around the PET film to form an impedance matching film according to Example 3. In this manner, a film with an impedance matching film according to Example 3 was obtained. Hastelloy is a registered trademark of Haynes International Inc. It is believed that oxygen was detected in the impedance matching film according to Example 3 due to the influence of a small amount of residual oxygen that was taken into the chamber during sputtering.

[0083] A sample according to Example 3 was produced in the same manner as in Example 1, except that the impedance matching film according to Example 3 was used instead of the impedance matching film according to Example 1.

[0084] <Example 4> An impedance matching film according to Example 4 was formed on a PET film having a thickness of 23 μm by sputtering using a target material consisting of Cu (copper), Ni (nickel), and Si (silicon) while supplying argon gas around the PET film.

[0085] A sample according to Example 4 was produced in the same manner as in Example 1, except that the impedance matching film according to Example 4 was used instead of the impedance matching film according to Example 1.

[0086] <Example 5> An impedance matching film according to Example 5 was formed on a PET film having a thickness of 23 μm by sputtering using a target material consisting of Cu (copper), Ni (nickel), and Si (silicon) while supplying argon gas around the PET film.

[0087] A sample according to Example 5 was produced in the same manner as in Example 1, except that the impedance matching film according to Example 5 was used instead of the impedance matching film according to Example 1.

[0088] <Example 6> An impedance matching film according to Example 6 was formed on a PET film having a thickness of 23 μm by sputtering using a target material consisting of Cu (copper), Ti (titanium), and Si (silicon) while supplying argon gas around the PET film.

[0089] A sample according to Example 6 was produced in the same manner as in Example 1, except that the impedance matching film according to Example 6 was used instead of the impedance matching film according to Example 1.

[0090] <Example 7> An impedance matching film according to Example 7 was formed on a PET film having a thickness of 23 μm by sputtering using a target material consisting of Cu (copper), Ti (titanium), and Si (silicon) while supplying argon gas around the PET film.

[0091] A sample according to Example 7 was produced in the same manner as in Example 1, except that the impedance matching film according to Example 7 was used instead of the impedance matching film according to Example 1.

[0092] <Example 8> On a PET film having a thickness of 23 μm, a target material consisting of Ti (titanium) and Mo (molybdenum) was used to perform sputtering while supplying argon gas and nitrogen gas to the periphery of the PET film, to form an impedance matching film according to Example 8. It is believed that oxygen was detected in the impedance matching film according to Example 8 due to the influence of a small amount of residual oxygen that was taken into the chamber during sputtering.

[0093] A sample according to Example 8 was produced in the same manner as in Example 1, except that the impedance matching film according to Example 8 was used instead of the impedance matching film according to Example 1.

[0094] <Example 9> On a PET film having a thickness of 23 μm, a target material consisting of Ti (titanium) and Mo (molybdenum) was used, and sputtering was performed while supplying argon gas and nitrogen gas to the periphery of the PET film to form an impedance matching film according to Example 9. It is believed that oxygen was detected in the impedance matching film according to Example 9 due to the influence of a small amount of residual oxygen that was taken into the chamber during sputtering.

[0095] A sample according to Example 9 was produced in the same manner as in Example 1, except that the impedance matching film according to Example 9 was used instead of the impedance matching film according to Example 1.

[0096] <Example 10> On a PET film having a thickness of 23 μm, a target material consisting of Ti (titanium) and Mo (molybdenum) was used to perform sputtering while supplying argon gas and nitrogen gas to the periphery of the PET film, to form an impedance matching film according to Example 10. It is believed that oxygen was detected in the impedance matching film according to Example 10 due to the influence of a small amount of residual oxygen that was taken into the chamber during sputtering.

[0097] A sample according to Example 10 was produced in the same manner as in Example 1, except that the impedance matching film according to Example 10 was used instead of the impedance matching film according to Example 1.

[0098] <Comparative Example 1> On a PET film having a thickness of 23 μm, a target material containing Fe (iron), Cr (chromium), and Ni (nickel) was used, and sputtering was performed while supplying argon gas to the periphery of the PET film, to form an impedance matching film according to Comparative Example 1. In this manner, a film with an impedance matching film according to Comparative Example 1 was obtained.

[0099] A sample according to Comparative Example 1 was produced in the same manner as in Example 1, except that the impedance matching film according to Comparative Example 1 was used instead of the impedance matching film according to Example 1.

[0100] <Comparative Example 2> On a PET film having a thickness of 23 μm, a target material consisting of Ti (titanium) and Mo (molybdenum) was used, and sputtering was performed while supplying argon gas around the PET film to form an impedance matching film according to Comparative Example 2. It is believed that nitrogen and oxygen were detected in the impedance matching film according to Comparative Example 2 due to the influence of slight residual nitrogen and residual oxygen that were taken into the chamber during sputtering.

[0101] A sample according to Comparative Example 2 was produced in the same manner as in Example 1, except that the impedance matching film according to Comparative Example 2 was used instead of the impedance matching film according to Example 1.

[0102] As shown in Table 1, the sheet resistance change rate Cs of the impedance matching films according to Examples 1 to 10 was 20% or less. In contrast, the sheet resistance change rate Cs of the impedance matching films according to Comparative Examples 1 and 2 was 63% and 59%, respectively. This suggests that the sheet resistance of the impedance matching films according to Examples 1 to 10 is unlikely to change even when the impedance matching films are exposed to a high-temperature environment.

[0103] As shown in Table 2, the samples according to Examples 1 to 10 exhibited good radio wave absorbing performance.

[0104] [Table 1]

[0105] [Table 2] [Explanation of symbols]

[0106] 1a, 1b, 1c, 1d Radio wave absorber 10 Impedance matching film for radio wave absorber 15 Impedance-matching film for radio wave absorbers 20 Dielectric layer 30 Conductors 40b adhesive layer 50a, 50b Laminate for radio wave absorber

Claims

1. Contains a metal element and a non-metal element, It has a thickness of 10 to 200 nm, having a sheet resistance of 200 Ω / □ or more; The content of oxygen atoms based on the atomic number is less than 50%, The content of the nonmetallic elements based on the atomic number is 24 to 67%; Impedance matching film for radio wave absorbers.

2. 0.4 x 10 -3 2. The impedance matching film for a radio wave absorber according to claim 1, which has a resistivity of Ω·cm or more.

3. 3. The impedance matching film for a radio wave absorber according to claim 1, wherein the nonmetallic element is at least one element selected from the group consisting of B, C, N, O, F, Si, S, and Ge.

4. The impedance matching film for a radio wave absorber according to any one of claims 1 to 3, wherein the metal element is at least one element selected from the group consisting of Ni, Cr, Ti, W, Mo, Cu, Al, Sn, Pd, Ta, Rh, Au, Mg, Fe, Mn, Co, and V.

5. 5. The impedance matching film for a radio wave absorber according to claim 1, wherein the metal element is at least one element selected from the group consisting of Ni, Cr, Mo, and Ti.

6. 6. The impedance matching film for a radio wave absorber according to claim 5, wherein the total content of Ni, Cr, Mo and Ti based on the atomic number is 10% or more.

7. 7. The impedance matching film for a radio wave absorber according to claim 1, having a sheet resistance of 600 Ω / □ or less.

8. 8.0 x 10 -3 8. The impedance matching film for a radio wave absorber according to claim 1, having a resistivity of Ω·cm or less.

9. A substrate; The impedance matching film for a radio wave absorber according to any one of claims 1 to 8, Impedance matching film for radio wave absorbers.

10. An impedance matching film for a radio wave absorber according to any one of claims 1 to 8, A conductor that reflects radio waves; a dielectric layer disposed between the impedance matching film for the radio wave absorber and the conductor in a thickness direction of the impedance matching film for the radio wave absorber; Radio wave absorber.

11. An impedance matching film for a radio wave absorber according to any one of claims 1 to 8, a dielectric layer arranged in contact with the impedance matching film for the radio wave absorber in a thickness direction of the impedance matching film for the radio wave absorber; Laminate for radio wave absorber.

Citation Information

Patent Citations

  • RESISTANCE FILM FOR λ / 4 TYPE RADIO WAVE ABSORBER AND λ / 4 TYPE RADIO WAVE ABSORBER

    JP2018056562A

  • Electromagnetic wave absorber

    JP2018098367A

  • Λ / 4 type radio wave absorber

    WO2019182002A1