Grease composition

A grease composition with a balanced blending ratio of MoDTC and ZnDTP addresses the challenge of simultaneous friction and wear resistance, achieving effective lubricity under harsh conditions.

JP7575324B2Active Publication Date: 2024-10-29SUMICO LUBRICANT
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021053042
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-26
Publication Date
2024-10-29
Estimated Expiration
2041-03-26

AI Technical Summary

Technical Problem

Existing grease compositions struggle to balance friction resistance and wear resistance, with additives like zinc dithiophosphate providing wear resistance but not friction reduction, and molybdenum compounds reducing friction but not effectively preventing wear, and their combination leading to film formation inhibition.

Method used

A grease composition is formulated with a specific blending ratio of molybdenum dithiocarbamate (MoDTC) and zinc dialkyldithiophosphate (ZnDTP) within a range of 0.5 to 2.0 weight ratio, enhancing both friction and wear resistance by optimizing film formation on friction surfaces.

Benefits of technology

The composition achieves reduced friction and suppressed wear, demonstrating improved lubricity under severe operating conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575324000001
    Figure 0007575324000001
  • Figure 0007575324000002
    Figure 0007575324000002
Patent Text Reader

Abstract

To provide a grease composition which has friction resistance and also is excellent in wear resistance.SOLUTION: A grease composition comprises: a base grease including a base oil and a thickener; and molybdenum dithiocarbamate (MoDTC) and zinc dialkyldithiophosphate (ZnDTP) which are incorporated into the base grease. An incorporation rate of MoDTC (in an amount in terms of molybdenum) to ZnDTP (in an amount in terms of zinc) is 0.5 to 2.0 in a weight ratio.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a grease composition having friction resistance and excellent wear resistance. [Background technology]

[0002] Grease is mainly used for plain bearings, rolling bearings, or sliding surfaces where it is difficult to keep a film of lubricant attached due to the movement of the contact surface. Grease is usually prepared by blending a thickener and, if necessary, additives with a lubricating base oil.

[0003] In recent years, with the advancement of mechanical technology in automobiles, electrical equipment, etc., various devices tend to be smaller, lighter, more powerful, and have a longer life, and the operating conditions are becoming more severe. Accordingly, the required performance, such as lubricity, of the grease used in various devices is also increasing.

[0004] In order to improve the lubrication of grease, various selections of base oil, thickener, and additives have been proposed. For example, anti-wear agents such as phosphate esters and zinc dithiophosphates, friction control agents such as molybdenum compounds, oiliness improvers such as long-chain fatty acid esters and fatty acid amides, and extreme pressure agents such as organic sulfur and organic halogen compounds are commonly used for the purpose of improving friction resistance and wear resistance.

[0005] However, for example, zinc compounds such as the above-mentioned zinc dithiophosphate are excellent in imparting wear resistance but are unable to simultaneously achieve a friction reducing effect, and molybdenum compounds, which are friction control agents, are highly effective in reducing friction but are poor in preventing wear and are also problematic as they can cause sludge.

[0006] Furthermore, as a result of research by the present inventors, it was found that the combined use of MoDTP (molybdenum dithiocarbamate), a friction control agent, and ZnDTP (dialkyldithiophosphate), an anti-wear agent, may inhibit the formation of Mo and Zn films on the coating surface.As driving conditions become more severe and further performance improvements are required, there are still challenges to be overcome in developing a grease composition that combines friction resistance and wear resistance. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2008-101122 A [Patent Document 2] JP 2016-044265 A [Patent Document 3] JP 2006-45264 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a grease composition that has both friction resistance and excellent wear resistance. [Means for solving the problem]

[0009] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result have found that it is possible to achieve both friction resistance and wear resistance by adjusting the blending ratio of MoDTP and ZnDTP, which are blended as additives, in a grease composition within a specific range, thereby completing the present invention.

[0010] (1) A first aspect of the present invention is a grease composition comprising a base grease containing a base oil and a thickener, molybdenum dithiocarbamate (MoDTC) and zinc dialkyldithiophosphate (ZnDTP), and the blending ratio of MoDTC (in molybdenum equivalent) to ZnDTP (in zinc equivalent) is 0.5 to 2.0 by weight. Effect of the Invention

[0011] According to the present invention, it is possible to provide a grease composition that has both friction resistance and excellent wear resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] A specific embodiment of the present invention (hereinafter, referred to as the present embodiment) will be described in detail below. Note that the present invention is not limited to the following embodiment, and can be appropriately modified within the scope of the present invention.

[0013] 1. Grease composition The grease composition according to the present embodiment is obtained by blending molybdenum dithiocarbamate (MoDTC) and zinc dialkyldithiophosphate (ZnDTP) with a base grease containing a base oil and a thickener. The grease composition is characterized in that the blending ratio of nDTP (zinc equivalent) to MoDTC (molybdenum equivalent) is 0.5 to 2.0 by weight.

[0014] [Base oil] Base oil is the main component of grease and constitutes the base grease together with a thickener, which will be described later.

[0015] The base oil is not particularly limited, and may be one that has been generally used. For example, lubricating oils such as mineral oil, ether oil-based synthetic oil, ester oil-based synthetic oil, and hydrocarbon synthetic oil, or synthetic oils thereof may be used. Among them, it is preferable to use ester oil-based synthetic oil and hydrocarbon synthetic oil. Examples of the ester oil-based synthetic oil include polyol ester oil, phosphate ester oil, polymer ester oil, aromatic ester oil, carbonate ester oil, diester oil, and polyglycol oil. Examples of the hydrocarbon synthetic oil include poly-α-olefin (PAO).

[0016] The base oil may be used alone or in combination of two or more kinds. For example, two or more kinds of base oils having different viscosities may be used in combination to constitute the base oil.

[0017] The content of the base oil in the grease composition is not particularly limited, and can be determined in consideration of the blending ratio with the thickener described below that constitutes the base grease. For example, the content in the composition can be 50% by mass or more, preferably 60% by mass or more, and more preferably 70% by mass or more. The upper limit is not particularly limited, and may be set within a range that does not impair the effects of the blending components described below, for example, about 95% by mass or less.

[0018] [Thickener] The thickener is a material necessary for retaining oil in the grease, and constitutes the base grease together with the base oil. The thickener is not particularly limited, and any conventionally used thickener can be used.

[0019] Specifically, thickeners can be broadly classified into soap-based and non-soap-based, and examples of the soap-based thickeners include lithium soap, lithium complex soap, calcium soap, calcium complex soap, aluminum soap, and aluminum complex soap, while examples of the non-soap-based thickeners include urea, sodium terephthalate, fluororesin, organic bentonite, silica gel, etc. These thickeners can be used alone or in combination of two or more.

[0020] The content of the thickener in the grease composition is not particularly limited, and can be determined taking into consideration the blending ratio of the above-mentioned base oil constituting the base grease.

[0021] [Molybdenum dithiocarbamate (MoDTC)] The grease composition according to the present embodiment contains molybdenum dithiocarbamate (hereinafter referred to as "MoDTC").

[0022] MoDTC is an organic molybdenum compound that acts as a friction modifier (reducer). MoDTC forms a film of molybdenum disulfide (Mo2S) made of layered crystals due to friction on the friction surface to which grease is applied, and this film reduces friction.

[0023] Specifically, examples of MoDTC include molybdenum sulfide diethyl dithiocarbamate, molybdenum sulfide dipropyl dithiocarbamate, molybdenum sulfide dibutyl dithiocarbamate, molybdenum sulfide dipentyl dithiocarbamate, molybdenum sulfide dihexyl dithiocarbamate, molybdenum sulfide dioctyl dithiocarbamate, molybdenum sulfide didecyl dithiocarbamate, molybdenum sulfide didodecyl dithiocarbamate, molybdenum sulfide di(butylphenyl)dithiocarbamate, molybdenum sulfide di(nonylphenyl)dithiocarbamate, and oxymolybdenum sulfide diethyl dithiocarbamate. oxymolybdenum sulfide dipropyl dithiocarbamate, oxymolybdenum sulfide dibutyl dithiocarbamate, oxymolybdenum sulfide dipentyl dithiocarbamate, oxymolybdenum sulfide dihexyl dithiocarbamate, oxymolybdenum sulfide dioctyl dithiocarbamate, oxymolybdenum sulfide didecyl dithiocarbamate, oxymolybdenum sulfide didodecyl dithiocarbamate, oxymolybdenum sulfide di(butylphenyl)dithiocarbamate, oxymolybdenum sulfide di(nonylphenyl)dithiocarbamate, and mixtures thereof.

[0024] The amount of MoDTC in the grease composition is not particularly limited as long as the weight ratio to zinc dialkyldithiophosphate (ZnDTP) described later is within a specific range. Specifically, the amount is preferably 1000 ppm or more, more preferably 2000 ppm or more, and particularly preferably 3000 ppm or more, calculated as molybdenum.

[0025] [Zinc dialkyldithiophosphate (ZnDTP)] The grease composition according to the present embodiment contains zinc dialkyldithiophosphate (hereinafter referred to as "ZnDTP").

[0026] ZnDTP is a compound represented by the following general formula, and acts as an anti-wear agent. ZnDTP forms a zinc phosphate film through friction on a friction surface coated with grease, and this film reduces wear.

[0027] [ka]

[0028] In the above general formula, R 1 ~R 4 are hydrocarbon groups (alkyl groups) and may be the same or different. For example, R 1 ~R 4Examples of the aryl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, a secondary butyl group, an isobutyl group, a pentyl group, a 4-methylpentyl group, a hexyl group, a 2-ethylhexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an isodecyl group, a dodecyl group, a tetradecyl group, a hexadecyl group, an octadecyl group, an eicosyl group, a docosyl group, a tetracosyl group, a cyclopentyl group, a cyclohexyl group, a methylcyclohexyl group, an ethylcyclohexyl group, a dimethylcyclohexyl group, a cycloheptyl group, a phenyl group, a tolyl group, a xylyl group, an ethylphenyl group, a propylphenyl group, a butylphenyl group, a pentylphenyl group, a hexylphenyl group, a heptylphenyl group, an octylphenyl group, a nonylphenyl group, a decylphenyl group, a dodecylphenyl group, a tetradecylphenyl group, a hexadecylphenyl group, an octadecylphenyl group, and a benzyl group.

[0029] The amount of ZnDTP in the grease composition is not particularly limited as long as the weight ratio to MoDTC is within a specific range. Specifically, the amount is preferably 500 ppm or more, more preferably 3000 ppm or more, and particularly preferably 6000 ppm or more, calculated as zinc.

[0030] [Weight ratio of MoDTC to ZnDTP] In the grease composition according to the present embodiment, the blending ratio of MoDTC (equivalent to molybdenum) to ZnDTP (equivalent to zinc) is 0.5 to 2.0 by weight.

[0031] As a result of the study by the present inventor, it was found that the blending ratio of MoDTC to ZnDTP affects the formation of each of the molybdenum disulfide coating (hereinafter also referred to as "Mo film") and zinc phosphate coating (hereinafter also referred to as "Zn film"). That is, in a grease composition, if the blending ratio of MoDTC to ZnDTP is too large, the Mo film inhibits the formation of the Zn film, while, on the other hand, if the blending ratio of ZnDTP to MoDTC is too large, the Zn film inhibits the formation of the Mo film, and unexpectedly, the Zn film itself is not formed sufficiently. From this, it was found that it is important to set the blending ratio of MoDTC to ZnDTP within a specific range in order to realize low friction while suppressing wear on the friction surface to which the grease composition is applied.

[0032] Specifically, as described above, the blending ratio of MoDTC to ZnDTP is set to a range of 0.5 to 2.0 in terms of weight ratio (hereinafter also referred to as "Mo / Zn ratio"). If the Mo / Zn ratio is greater than 2.0, the formation of the Zn film is inhibited, and wear cannot be effectively suppressed. If the Mo / Zn ratio is less than 0.5, the formation of the Mo film is inhibited, and friction cannot be effectively reduced. Furthermore, the Zn film itself is not sufficiently formed, and wear cannot be suppressed.

[0033] Regarding the Mo / Zn ratio, the lower limit is preferably 0.7 or more, and more preferably 1.0 or more, and the upper limit is preferably 1.8 or less, and more preferably 1.5 or less.

[0034] [others] In the grease composition according to the present embodiment, in addition to the above-mentioned components, various additives generally used in lubricating oils and greases, such as extreme pressure agents, antioxidants, rust inhibitors, polymer additives, etc., can be blended as necessary. In addition to the above-mentioned components, additives such as friction modifiers, anti-wear agents, and solid lubricants can also be added. When these additives are added, the content of each is preferably about 0.1% by mass to 10% by mass of the total amount of the grease composition.

[0035] Needless to say, the above-mentioned additives may be contained as components constituting the base grease together with the base oil and the thickener.

[0036] 2. Method for producing grease composition As described above, the grease composition according to the present embodiment is made by blending molybdenum dithiocarbamate (MoDTC) and zinc dialkyldithiophosphate (ZnDTP) with a base grease containing a base oil and a thickener, and the blending ratio of nDTP (zinc equivalent) to MoDTC (molybdenum equivalent) is 0.5 to 2.0 by weight. This grease composition can be produced by a well-known method, like conventional grease compositions.

[0037] Specifically, for example, a base grease is prepared by kneading a base oil with a thickener such as a metal soap, and then MoDTC and ZnDTP are added to and dispersed in a predetermined blend ratio in the base grease, and various additives are further added as necessary and kneaded to obtain the composition.

[0038] The kneading treatment can be carried out using a well-known stirring / dispersing treatment device such as a three-roll mill, a universal mixer, a homogenizer, a colloid mill, etc. Note that the kneading is not limited to the above-mentioned process of adding each component in order, and each component may be added and kneaded simultaneously. EXAMPLES

[0039] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0040] [Production of grease composition] In the examples and comparative examples, grease compositions were produced so as to have the compositions shown in Table 1 below. Specifically, a certain amount of base oil and fatty acid were weighed into a beaker, and heated while stirring until the fatty acid melted. An alkali was used to cause primary and secondary saponification reactions, and after completely removing water, the temperature was raised to a predetermined temperature, and then naturally cooled to produce a base grease. Next, the produced base grease, MoDTC, and ZnDTP were weighed, and subjected to stirring and dispersion treatments to produce a grease composition. Stirring was performed using a universal stirrer. Dispersion treatment was also performed using a three-roll mill. Note that mineral oil and polyalphaolefin (PAO) were used as the base oil, and a base grease containing lithium complex soap as a thickener was produced as described above.

[0041] [Evaluation test] (SRV Test) A lubricity test was carried out on the prepared grease composition using an SRV tester under the following test conditions. The average friction coefficient for 30 minutes was measured by this test. The wear scar diameter was also measured based on the wear scar formed. Tester: SRV tester Contact type: Ball-on-disk Test piece: Ball SUJ-2 (φ10mm) Disk SUJ-2 (φ24.0×7.9mm) Grease application amount: 80μm (film thickness) Load: 80N ·Amplitude: 1.5mm Vibration frequency: 50Hz ·Temperature: 80℃ Duration: 180 minutes

[0042] [result] Table 1 below shows the composition of the grease composition and the evaluation results.

[0043] [Table 1]

[0044] As can be seen from the results shown in Table 1, in the examples in which the weight ratio of MoDTC (equivalent to molybdenum) and ZnDTP (equivalent to zinc) in the grease composition was 0.5 to 2.0, the friction coefficient was effectively reduced, and the wear scar was small, effectively suppressing wear.

[0045] In contrast, in Comparative Example 3, where Mo / Zn was 0.2, the friction coefficient was larger than in the Examples, and the wear marks were also larger. In Comparative Example 4, where Mo / Zn was 3.0, the friction coefficient was kept low, but wear could not be suppressed and large wear marks were formed. Furthermore, in Comparative Examples 5 to 7, where Mo / Zn was 4.0 or more, the friction coefficient was larger and the wear marks were also larger. The results of these Comparative Examples are considered to be due to the inhibition of the formation of Mo and Zn films on the friction surface.

[0046] Here, in Comparative Example 2, since the grease composition was blended with only MoDTC, the friction coefficient was reduced, but since ZnDTP was not blended, wear occurred and a large wear scar diameter was formed. On the other hand, the grease composition of Comparative Example 3, which was blended with ZnDTP, unexpectedly had a large wear scar diameter equivalent to that of Comparative Example 2, and wear could not be effectively suppressed. This is thought to be because the MoDTC content was low and Mo / Zn was less than 0.5, so that the Zn film was not sufficiently formed.

Claims

[Claim 1] A base grease containing a base oil and a thickener, Molybdenum dithiocarbamate (MoDTC) and zinc dialkyldithiophosphate (ZnDTP) are blended. The blending ratio of the MoDTC (equivalent amount of molybdenum) to the ZnDTP (equivalent amount of zinc) is 0.5 to 2.0 by weight, The amount of ZnDTP blended is 3000 ppm or more in terms of zinc; Grease composition.

Citation Information

Patent Citations

  • Grease composition for constant velocity joint

    JP1996041485A

  • Grease composition for uniform joint

    JP1996120289A

  • Grease composition for constant velocity joint

    JP1998273691A

  • Lubricating composition containing friction-reducing additive package and grease

    JP2001520301A

  • Grease composition and rolling device

    JP2006045264A