Copolymer, rubber composition and resin composition

A copolymer with high non-conjugated olefin units and tailored crystallinity addresses the lack of cut and ozone resistance in rubber and resin products, providing enhanced durability and performance.

JP7575928B2Active Publication Date: 2024-10-30BRIDGESTONE CORP
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2020203021
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-07
Publication Date
2024-10-30
Estimated Expiration
2040-12-07

AI Technical Summary

Technical Problem

Existing rubber and resin products lack both cut resistance and ozone resistance, as highlighted by the limitations in Patent Document 1, which does not focus on these properties.

Method used

A copolymer with a high proportion of non-conjugated olefin units (50 mol% or more) and specific crystallinity characteristics, combined with conjugated diene units, enhances cut resistance and ozone resistance. The copolymer includes a crystallinity of 13% or more, a melting point of 100°C or higher, and a weight average molecular weight of 50,000 to 2,000,000, ensuring mechanical strength and workability.

Benefits of technology

The copolymer exhibits excellent cut resistance and ozone resistance, improving the durability and performance of rubber and resin compositions by enhancing their ability to withstand cuts and resist ozone degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575928000017
    Figure 0007575928000017
  • Figure 0007575928000018
    Figure 0007575928000018
  • Figure 0007575928000019
    Figure 0007575928000019
Patent Text Reader

Abstract

To provide a copolymer excellent in cutting resistance and ozone resistance.SOLUTION: The copolymer has a conjugated diene unit and a non-conjugated olefin unit, the proportion of the non-conjugated olefin unit is 50 mol% or more, and the crystallinity (C2) within the range of 100°C or higher and 150°C or lower is larger than the crystallinity (C1) within the range of 0°C or higher and lower than 100°C when measured by a differential scanning calorimeter (DSC).SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a copolymer, a rubber composition, and a resin composition. [Background technology]

[0002] When two or more types of monomers are polymerized in the same reaction system, a copolymer is produced in which units of those monomers are contained in a single polymer chain.

[0003] For example, Patent Document 1 discloses a copolymer of a conjugated diene compound and a non-conjugated olefin as a copolymer having excellent wet properties and low-temperature properties, in which the amount of 1,2-vinyl bonds is 10 mol% or more and the amount of cis-1,4 bonds is 50 to 90 mol% relative to the total amount of conjugated diene units derived from the conjugated diene compound, and the content of non-conjugated olefin units derived from the non-conjugated olefin in the copolymer is 18 mol% to 45 mol%. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-131965 A Summary of the Invention [Problem to be solved by the invention]

[0005] On the other hand, rubber products (tires, conveyor belts, anti-vibration rubber, seismic isolation rubber, etc.) and resin products are often required to have both cut resistance and ozone resistance, and it would be useful to develop a polymer or copolymer that satisfies such requirements. However, Patent Document 1 does not pay attention to either cut resistance or ozone resistance.

[0006] Therefore, an object of the present invention is to provide a copolymer having excellent cut resistance and ozone resistance. Another object of the present invention is to provide a rubber composition and a resin composition which contain the copolymer and have excellent cut resistance and ozone resistance. [Means for solving the problem]

[0007] The gist of the present invention for solving the above problems is as follows.

[0008] The copolymer of the present invention is a copolymer having conjugated diene units and non-conjugated olefin units, The proportion of the non-conjugated olefin units is 50 mol % or more, It is characterized in that the degree of crystallinity (C2) in the range of 100°C or higher and 150°C or lower, as measured by a differential scanning calorimeter (DSC), is greater than the degree of crystallinity (C1) in the range of 0°C or higher and lower than 100°C. Such a copolymer of the present invention is excellent in cut resistance and ozone resistance.

[0009] The copolymer of the present invention preferably has a crystallinity (C2) of 13% or more within the above-mentioned range of 100° C. to 150° C. In this case, cut resistance can be improved more efficiently.

[0010] The copolymer of the present invention preferably has a crystallinity (C1) of less than 13% in the range of from 0° C. to less than 100° C. In this case, cut resistance can be improved more efficiently.

[0011] In the copolymer of the present invention, the proportion of the conjugated diene units is preferably 5 mol % or more and less than 50 mol %, and the proportion of the non-conjugated olefin units is preferably 50 mol % or more and 95 mol % or less, which can further improve cut resistance and ozone resistance.

[0012] The copolymer of the present invention preferably has a melting point measured by a differential scanning calorimeter (DSC) of 100° C. or higher, in which case cut resistance can be improved more efficiently.

[0013] The copolymer of the present invention preferably has a weight average molecular weight in terms of polystyrene of 50,000 to 2,000,000, which can ensure sufficient mechanical strength and maintain high workability.

[0014] The copolymer of the present invention preferably has an endothermic peak energy of 35 J / g or more as measured by a differential scanning calorimeter (DSC), which can more sufficiently improve cut resistance.

[0015] In the copolymer of the present invention, from the viewpoint of further improving the ozone resistance, the non-conjugated olefin unit is preferably an acyclic non-conjugated olefin unit.

[0016] In the copolymer of the present invention, from the viewpoint of further improving the ozone resistance, the non-conjugated olefin units preferably consist of only ethylene units.

[0017] In the copolymer of the present invention, from the viewpoint of effectively improving durability including cut resistance, the conjugated diene units preferably contain 1,3-butadiene units and / or isoprene units.

[0018] The copolymer of the present invention may further contain the aromatic vinyl unit.

[0019] The rubber composition of the present invention is characterized by containing the above-mentioned copolymer of the present invention. The rubber composition of the present invention is excellent in cut resistance and ozone resistance.

[0020] The rubber composition of the present invention preferably further contains a compound having two or more phenyl groups each having a branched alkyl group as an antiaging agent, which can improve the dispersibility of the copolymer and inhibit the copolymer from gelling.

[0021] The resin composition of the present invention is characterized by containing the above-mentioned copolymer of the present invention. The resin composition of the present invention is excellent in cut resistance and ozone resistance.

[0022] The resin composition of the present invention preferably further contains a compound having two or more phenyl groups each having a branched alkyl group as an antioxidant, which can improve the dispersibility of the copolymer and inhibit the copolymer from gelling. Effect of the Invention

[0023] According to the present invention, a copolymer having excellent cut resistance and ozone resistance can be provided. Moreover, according to the present invention, it is possible to provide a rubber composition and a resin composition that are excellent in cut resistance and ozone resistance. [Brief description of the drawings]

[0024] [Figure 1] 1 is a DSC chart of the copolymer of Example 1. [Diagram 2] 1 is a DSC chart of the copolymer of Example 2. [Diagram 3] 1 is a DSC chart of the copolymer of Example 3. [Figure 4] 1 is a DSC chart of the copolymer of Example 4. [Diagram 5] 1 is a DSC chart of the copolymer of Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0025] The copolymer, rubber composition, and resin composition of the present invention will be illustrated in detail below based on embodiments.

[0026] (copolymer) A copolymer according to one embodiment of the present invention (hereinafter, sometimes referred to as "the copolymer of the present embodiment") is a copolymer having conjugated diene units and non-conjugated olefin units, wherein the proportion of the non-conjugated olefin units is 50 mol% or more, and the degree of crystallinity (C2) in the range of 100°C or more and 150°C or less, measured by differential scanning calorimetry (DSC), is greater than the degree of crystallinity (C1) in the range of 0°C or more and less than 100°C.

[0027] As described above, the copolymer has a ratio of non-conjugated olefin units of 50 mol% or more, so that the amount of double bonds derived from diene components such as conjugated diene compounds is small, and as a result, ozone resistance can be improved. Also, as described above, the copolymer has a crystallinity (C2) in the range of 100°C to 150°C measured by differential scanning calorimetry (DSC) that is greater than the crystallinity (C1) in the range of 0°C to less than 100°C (C2>C1). Thus, the fact that the crystallinity is higher on the high temperature side than on the low temperature side with 100°C as the boundary means that the chain derived from the non-conjugated olefin compound is longer. And, due to such a long chain, crystal melting energy is generated when impact such as cutting is received, so that cut resistance can be improved.

[0028] When the proportion of non-conjugated olefin units in the copolymer is less than 50 mol %, even if C2>C1, it is believed that at least one of the ozone resistance and cut resistance becomes insufficient.

[0029] The degree of crystallinity (C1) of the copolymer in the range of 0°C to less than 100°C can be determined by measuring the endothermic peak energy (ΔH1 (J / g)) in the range of 0°C to less than 100°C using a differential scanning calorimeter (DSC) and measuring the crystalline melting energy (ΔH0) of the polyethylene of 100% crystalline component, and calculating the ratio (ΔH1 / ΔH0). Similarly, the degree of crystallinity (C2) of the copolymer in the range of 100°C to 150°C can be determined by measuring the endothermic peak energy (ΔH2 (J / g)) in the range of 100°C to 150°C using a differential scanning calorimeter (DSC) and calculating the ratio (ΔH2 / ΔH0) to the crystalline melting energy (ΔH0).

[0030] The copolymer of the present embodiment preferably has a crystallinity (C1) of less than 13% in the range of 0°C or more and less than 100°C. In this case, the proportion of short chain portions in the entire portion derived from the non-conjugated olefin compound in the copolymer is reduced, and cut resistance can be improved more efficiently. From the same viewpoint, the crystallinity (C1) of the copolymer in the range of 0°C or more and less than 100°C is more preferably 10% or less, even more preferably 8% or less, even more preferably 7% or less, and particularly preferably 0%.

[0031] The copolymer of the present embodiment preferably has a crystallinity (C2) of 13% or more in the range of 100°C to 150°C. In this case, the proportion of long chain parts in the entire part derived from the non-conjugated olefin compound in the copolymer increases, and cut resistance can be improved more efficiently. From the same viewpoint, the crystallinity (C2) of the copolymer in the range of 100°C to 150°C is more preferably 15% or more, and further preferably 20% or more. In addition, the upper limit of the crystallinity (C2) in the range of 100°C to 150°C is not particularly limited, but is preferably 60% or less from the viewpoint of maintaining good workability.

[0032] In the copolymer of the present embodiment, the ratio (C1 / C2) of the crystallinity (C1) in the range of 0°C or more and less than 100°C to the crystallinity (C2) in the range of 100°C or more and 150°C or less is preferably 0.60 or less. In this case, the proportion of long chain parts in the entire part derived from the non-conjugated olefin compound in the copolymer increases, and cut resistance can be improved more efficiently. From the same viewpoint, the ratio (C1 / C2) is more preferably 0.55 or less, even more preferably 0.50 or less, particularly preferably 0.45 or less, and even more particularly preferably 0.40 or less.

[0033] The copolymer of the present embodiment has at least a conjugated diene unit and a non-conjugated olefin unit as monomer units, and may consist of only a conjugated diene unit and a non-conjugated olefin unit, or may further have other monomer units.

[0034] The conjugated diene unit is a monomer unit derived from a conjugated diene compound. The conjugated diene unit enables crosslinking (vulcanization) of the copolymer, and can also exhibit elongation and strength as rubber. Here, the conjugated diene compound refers to a conjugated diene compound. The conjugated diene compound as a monomer of the copolymer preferably has 4 to 8 carbon atoms. Specific examples of such conjugated diene compounds include 1,3-butadiene, isoprene, 1,3-pentadiene, and 2,3-dimethyl-1,3-butadiene. The above conjugated diene compounds may be used alone or in combination of two or more kinds. From the viewpoint of effectively improving durability including cut resistance, the conjugated diene compound as a monomer of the copolymer preferably contains 1,3-butadiene and / or isoprene, more preferably consists of only 1,3-butadiene and / or isoprene, and even more preferably consists of only 1,3-butadiene. In other words, the conjugated diene units in the copolymer preferably contain 1,3-butadiene units and / or isoprene units, more preferably consist of only 1,3-butadiene units and / or isoprene units, and even more preferably consist of only 1,3-butadiene units.

[0035] The proportion of the conjugated diene unit in the copolymer is preferably 5 mol% or more, and is less than 50 mol%. When the proportion of the conjugated diene unit in the copolymer is 5 mol% or more, the elongation is excellent, and durability including cut resistance can be further improved. From the same viewpoint, the proportion of the conjugated diene unit in the copolymer is more preferably 10 mol% or more, and even more preferably 15 mol% or more. In addition, from the viewpoint of further improving ozone resistance, the proportion of the conjugated diene unit in the copolymer is preferably 45 mol% or less, more preferably 40 mol% or less, and even more preferably 35 mol% or less.

[0036] The non-conjugated olefin unit is a monomer unit derived from a non-conjugated olefin compound. The copolymer can have crystallinity by having the non-conjugated olefin unit. Here, the non-conjugated olefin compound refers to an aliphatic unsaturated hydrocarbon compound having one or more carbon-carbon double bonds. The non-conjugated olefin compound as a monomer of the copolymer preferably has 2 to 10 carbon atoms. Specific examples of such non-conjugated olefin compounds include α-olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene, and heteroatom-substituted alkene compounds such as vinyl pivalate, 1-phenylthioethene, and N-vinylpyrrolidone. The non-conjugated olefin compound may be a single type or a combination of two or more types. From the viewpoint of further improving ozone resistance, the non-conjugated olefin compound as a monomer of the copolymer is preferably an acyclic non-conjugated olefin compound, more preferably an α-olefin, even more preferably an α-olefin containing ethylene, and even more preferably consisting of ethylene alone. In other words, the non-conjugated olefin units in the copolymer are preferably acyclic non-conjugated olefin units, more preferably α-olefin units, even more preferably α-olefin units containing ethylene units, and even more preferably consisting of only ethylene units.

[0037] The proportion of non-conjugated olefin units in the copolymer is preferably 50 mol% or more and 95 mol% or less. If the proportion of non-conjugated olefin units in the copolymer is less than 50 mol%, there is a risk that ozone resistance is not sufficiently improved. On the other hand, if the proportion of non-conjugated olefin units in the copolymer is 95 mol% or less, the proportion of conjugated diene units increases, and the breaking properties (especially elongation at break (EB)) can be improved. From the same viewpoint, the proportion of non-conjugated olefin units in the copolymer is preferably 55 mol% or more, more preferably 60 mol% or more, even more preferably 65 mol% or more, and more preferably 90 mol% or less, even more preferably 85 mol% or less.

[0038] The copolymer preferably contains the conjugated diene unit in a proportion of 5 mol % or more and less than 50 mol %, and the non-conjugated olefin unit in a proportion of 50 mol % or more and 95 mol % or less, thereby making it possible to further improve cut resistance and ozone resistance.

[0039] As described above, the copolymer may have other monomer units other than the conjugated diene units and the non-conjugated olefin units. For example, the copolymer may further have an aromatic vinyl unit as the other monomer unit.

[0040] The aromatic vinyl unit is a monomer unit derived from an aromatic vinyl compound. Here, the aromatic vinyl compound refers to an aromatic compound substituted with at least a vinyl group, and is not included in the conjugated diene compound. The aromatic vinyl compound as a monomer of the copolymer preferably has 8 to 10 carbon atoms. Specific examples of such aromatic vinyl compounds include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, o-ethylstyrene, m-ethylstyrene, and p-ethylstyrene. The aromatic vinyl compound may be a single type or a combination of two or more types. The aromatic vinyl compound as a monomer of the copolymer preferably contains styrene, and more preferably consists of styrene only. In other words, the aromatic vinyl unit in the copolymer preferably contains a styrene unit, and more preferably consists of a styrene unit only. Incidentally, the aromatic ring in the aromatic vinyl unit is not included in the main chain of the copolymer unless it is bonded to an adjacent unit.

[0041] When the copolymer has aromatic vinyl units, the proportion of the aromatic vinyl units is preferably 1 mol% or more, and preferably 30 mol% or less. When the proportion of the aromatic vinyl units in the copolymer is 1 mol% or more, the fracture properties at high temperatures can be improved. When the proportion of the aromatic vinyl units in the copolymer is 30 mol% or less, the effects of the conjugated diene units and non-conjugated olefin units can be fully exhibited.

[0042] However, from the viewpoint of more reliably obtaining the desired effect, the proportion of the other monomer units in the copolymer is preferably 20 mol % or less of the entire copolymer, more preferably 10 mol % or less, even more preferably 5 mol % or less, and particularly preferably 0 mol % (i.e., the copolymer is composed only of conjugated diene units and non-conjugated olefin units).

[0043] The copolymer has a butylene unit ratio of 0 mol % (has no butylene units), that is, the copolymer does not include hydrogenated styrene-butadiene copolymers such as styrene-ethylene / butylene-styrene (SEBS).

[0044] The copolymer of the present embodiment may have a cyclic structure in the main chain, or may be composed only of a non-cyclic structure in the main chain. When the main chain has a non-cyclic structure, durability including cut resistance can be further improved. Incidentally, NMR is used as a main measurement means for confirming whether the main chain of a copolymer has a cyclic structure or not. Specifically, when a peak derived from a cyclic structure present in the main chain (for example, a peak appearing at 10 to 24 ppm for a three- to five-membered ring) is not observed, it indicates that the main chain of the copolymer is composed of only a non-cyclic structure. On the other hand, when the peak is observed, it indicates that the main chain has a cyclic structure.

[0045] The copolymer of the present embodiment preferably has an endothermic peak energy of 35 J / g or more as measured by a differential scanning calorimeter (DSC). If the endothermic peak energy is 35 J / g or more, the cut resistance can be more sufficiently improved. The endothermic peak energy is an endothermic peak energy in the range of 0 to 150°C. For example, when the endothermic peak energy is separately described as an endothermic peak energy of 0 to less than 100°C and an endothermic peak energy of 100°C to 150°C, the sum of these values ​​represents the degree of crystallinity in the range of 0 to 150°C.

[0046] The copolymer of the present embodiment preferably has an endothermic peak energy (ΔH2) of 35 J / g or more in the range of 100° C. to 150° C. If the endothermic peak energy (ΔH2) is 35 J / g or more in the range of 100° C. to 150° C., the proportion of long chain portions in the entire portion derived from the non-conjugated olefin compound in the copolymer increases, and cut resistance can be improved more efficiently.

[0047] The copolymer of the present embodiment preferably has a melting point of 100°C or higher as measured by a differential scanning calorimeter (DSC). If the melting point of the copolymer is 100°C or higher, the proportion of long chain portions in the entire portion derived from the non-conjugated olefin compound increases, and cut resistance can be improved more efficiently. From the same viewpoint, the melting point of the copolymer is more preferably 105°C or higher, further preferably 110°C or higher, and even more preferably 115°C or higher. In addition, the upper limit of the melting point of the copolymer is not particularly limited, but from the viewpoint of maintaining good workability, it is preferably 200°C or lower. The melting point is a value measured using a differential scanning calorimeter in accordance with JIS K 7121-1987.

[0048] The copolymer of the present embodiment preferably has a glass transition temperature of 0°C or lower as measured by a differential scanning calorimeter (DSC). If the glass transition temperature of the copolymer is 0°C or lower, workability is improved. From the same viewpoint, the glass transition temperature of the copolymer is more preferably -50°C or lower, further preferably -80°C or lower, and even more preferably -100°C or lower. In addition, the lower limit of the glass transition temperature of the copolymer is not particularly limited, but is preferably -150°C or higher. The glass transition temperature is a value measured using a differential scanning calorimeter in accordance with JIS K 7121-1987.

[0049] The copolymer of the present embodiment preferably has a polystyrene-equivalent weight average molecular weight (Mw) of 50,000 to 2,000,000. When the copolymer has an Mw of 50,000 or more, it is possible to ensure sufficient mechanical strength, and when the Mw is 2,000,000, it is possible to maintain high workability. From the same viewpoint, the Mw of the copolymer is more preferably 100,000 or more, and even more preferably 150,000 or more, and more preferably 1,000,000 or less, and even more preferably 800,000 or less.

[0050] The copolymer of the present embodiment preferably has a polystyrene-equivalent number average molecular weight (Mn) of 50,000 to 2,000,000. When the copolymer has an Mn of 50,000 or more, it is possible to ensure sufficient mechanical strength, and when the Mn is 2,000,000, it is possible to maintain high workability. From the same viewpoint, the Mn of the copolymer is more preferably 80,000 or more, even more preferably 100,000 or more, and more preferably 1,000,000 or less, even more preferably 500,000 or less, and particularly preferably 300,000 or less.

[0051] The copolymer of this embodiment preferably has a molecular weight distribution [Mw / Mn (weight average molecular weight / number average molecular weight)] of 1.00 to 4.00, more preferably 1.50 to 3.50, and even more preferably 1.80 to 3.00. If the molecular weight distribution of the copolymer is 4.00 or less, sufficient homogeneity can be achieved in the physical properties of the copolymer. From the same viewpoint, the molecular weight distribution of the copolymer is more preferably 3.50 or less, and even more preferably 3.00 or less. Moreover, the molecular weight distribution of the copolymer is more preferably 1.50 or more, and even more preferably 1.80 or more.

[0052] The weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) are determined by gel permeation chromatography (GPC) using polystyrene as a standard substance.

[0053] The copolymer of the present embodiment described above can be prepared, for example, by polymerizing a predetermined monomer using a catalyst component described later. In this case, it is important to comprehensively control the type and composition of the catalyst component, the ratio of each catalyst component to the amount (or pressure) of the monomer to be added, the timing of adding each monomer, the polymerization time, and the like.

[0054] <Preparation of Copolymer> The copolymer of the present embodiment can be produced through a process of polymerizing a conjugated diene compound, a non-conjugated olefin compound, and, if necessary, other monomers, and may further include a coupling process, a washing process, and other processes, if necessary.

[0055] As the polymerization method, any method can be used, such as solution polymerization, suspension polymerization, liquid phase bulk polymerization, emulsion polymerization, gas phase polymerization, solid phase polymerization, etc. When a solvent is used in the polymerization reaction, the solvent may be any solvent that is inert in the polymerization reaction, and examples of the solvent include toluene, cyclohexane, and normal hexane.

[0056] The polymerization process may be carried out in one step, or in two or more steps. The one-step polymerization process is a process in which all types of monomers to be polymerized, i.e., non-conjugated olefin compounds, conjugated diene compounds, and any other monomers, preferably non-conjugated olefin compounds and conjugated diene compounds, are reacted and polymerized at the same time. The multi-step polymerization process is a process in which a part or all of one or two types of monomers are first reacted to form a polymer (first polymerization step), and then the remaining type of monomer or the remainder of the one or two types of monomers are added and polymerized in one or more steps (second polymerization step to final polymerization step).

[0057] The polymerization temperature is not particularly limited, but is preferably in the range of -100°C to 200°C, and can be around room temperature. The pressure of the polymerization reaction is preferably in the range of 0.1 to 10.0 MPa in order to sufficiently incorporate the conjugated diene compound into the polymerization reaction system. The time spent on polymerization is preferably in the range of 1 second to 10 days, but can be appropriately selected depending on the type of polymerization catalyst, polymerization temperature, and other conditions. In particular, when the polymerization temperature is 25 to 80°C, the time is preferably in the range of 5 minutes to 500 minutes. In the polymerization of the conjugated diene compound, the polymerization may be terminated using a polymerization terminator such as methanol, ethanol, isopropanol, or the like.

[0058] The monomer raw materials may be added simultaneously or successively. When the monomer raw materials are introduced into the polymerization system, it is preferable to control the flow rate of each monomer raw material and add them continuously to the polymerization system (so-called metering). When a monomer raw material that is gaseous under the polymerization system conditions (for example, ethylene as a non-conjugated olefin compound under room temperature and normal pressure conditions) is used, it can be introduced into the polymerization reaction system at a predetermined pressure.

[0059] Here, the polymerization of the above monomers is preferably carried out in the presence of one or more of the following components (A) to (F). In addition, in the polymerization step, it is preferable to use one or more of the following components (A) to (F) as a catalyst component, but it is more preferable to use a combination of two or more of the following components (A) to (F) as a catalyst composition.

[0060] Component (A): a rare earth element compound or a reaction product of the rare earth element compound with a Lewis base (B) Component: Organometallic compound Component (C): Aluminoxane (D) Component: Ionic compound (E) Component: Halogen compound Component (F): A cyclopentadiene skeleton-containing compound selected from substituted or unsubstituted cyclopentadiene (a compound having a cyclopentadienyl group), substituted or unsubstituted indene (a compound having an indenyl group), and substituted or unsubstituted fluorene (a compound having a fluorenyl group) (hereinafter, sometimes simply referred to as a "cyclopentadiene skeleton-containing compound"). Components (A) to (F) will be described in detail below.

[0061] Examples of the rare earth compound or the reaction product of the rare earth compound and a Lewis base (component (A)) include a rare earth compound having a rare earth-carbon bond or a reaction product of the rare earth compound and a Lewis base (hereinafter also referred to as "component (A-1)"), and a rare earth compound not having a rare earth-carbon bond or a reaction product of the rare earth compound and a Lewis base (hereinafter also referred to as "component (A-2)").

[0062] Examples of the component (A-1) include compounds represented by the following general formula (I-1): [ka] [In the formula, M represents a lanthanoid element, scandium or yttrium, and Cp R each independently represents unsubstituted or substituted indenyl; R a ~R f each independently represents an alkyl group having 1 to 3 carbon atoms or a hydrogen atom, L represents a neutral Lewis base, and w represents an integer of 0 to 3; and a metallocene complex represented by the following general formula (I-2): [ka] [where M, Cp R , R a ~R f , L, and w are the same as those in formula (I-1); R g ~R l teeth, each independently represents an alkyl group having 1 to 3 carbon atoms or a hydrogen atom], a complex represented by the following general formula (II-1): [ka] [In the formula, M represents a lanthanoid element, scandium or yttrium, and Cp R each independently represents an unsubstituted or substituted indenyl, X' represents a hydrogen atom, a halogen atom, an alkoxy group, a thiolate group, an amino group, a silyl group, or a monovalent hydrocarbon group having 1 to 20 carbon atoms, L represents a neutral Lewis base, and w represents an integer of 0 to 3; and a metallocene complex represented by the following general formula (II-2): [ka] [where M, Cp R , X′, L, and w are the same as those in formula (II-1), and a complex represented by the following general formula (III): [ka] [In the formula, M represents a lanthanoid element, scandium or yttrium, and Cp R’ represents unsubstituted or substituted cyclopentadienyl, indenyl, or fluorenyl; X represents a hydrogen atom, a halogen atom, an alkoxy group, a thiolate group, an amino group, a silyl group, or a monovalent hydrocarbon group having 1 to 20 carbon atoms; L represents a neutral Lewis base; w represents an integer of 0 to 3; [B] - represents a non-coordinating anion].

[0063] In the complexes represented by the above general formulae (I-1), (I-2), (II-1) and (II-2), Cp R is unsubstituted indenyl or substituted indenyl. R is C9H 7-x R x or C9H 11-x R x Here, X is an integer of 0 to 7 or 0 to 11. Each R is preferably independently a hydrocarbyl group or a metalloid group. The carbon number of the hydrocarbyl group is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 8. Specific examples of the hydrocarbyl group include a methyl group, an ethyl group, a phenyl group, a benzyl group, and the like. On the other hand, examples of the metalloid of the metalloid group include germyl Ge, stannyl Sn, and silyl Si. The metalloid group preferably has a hydrocarbyl group, and the hydrocarbyl group of the metalloid group is the same as the above hydrocarbyl group. Specific examples of the metalloid group include a trimethylsilyl group, and the like. Specific examples of the substituted indenyl include 2-phenylindenyl, 2-methylindenyl, and the like. In addition, when the two Cp R may be the same or different from each other.

[0064] In the half metallocene cation complex represented by the above general formula (III), Cp R’represents unsubstituted or substituted cyclopentadienyl, indenyl, or fluorenyl, and among these, preferably represents unsubstituted or substituted indenyl.

[0065] In the general formula (III), Cp having the above cyclopentadienyl ring as a basic skeleton R’ is C5H 5-x R x Here, X is an integer of 0 to 5. Each R is preferably independently a hydrocarbyl group or a metalloid group. The number of carbon atoms in the hydrocarbyl group is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 8. Specific examples of the hydrocarbyl group include a methyl group, an ethyl group, a phenyl group, a benzyl group, and the like. On the other hand, examples of the metalloid of the metalloid group include germyl Ge, stannyl Sn, and silyl Si. The metalloid group preferably has a hydrocarbyl group, and the hydrocarbyl group of the metalloid group is the same as the above hydrocarbyl group. Specific examples of the metalloid group include a trimethylsilyl group, and the like. Cp having a cyclopentadienyl ring as a basic skeleton R’ Specifically, the following are exemplified: [ka] [In the formula, R represents a hydrogen atom, a methyl group, or an ethyl group.]

[0066] In the general formula (III), Cp having the above indenyl ring as a basic skeleton R’ is Cp in general formula (I-1) and (II-1) R The same definitions are used, and preferred examples are also similar.

[0067] In the general formula (III), Cp having the above fluorenyl ring as a basic skeleton R’ is C 13 H 9-x R x Or C 13 H 17-x R xHere, X is an integer of 0 to 9 or 0 to 17. Each R is preferably independently a hydrocarbyl group or a metalloid group. The carbon number of the hydrocarbyl group is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 8. Specific examples of the hydrocarbyl group include a methyl group, an ethyl group, a phenyl group, and a benzyl group. On the other hand, examples of the metalloid of the metalloid group include germyl Ge, stannyl Sn, and silyl Si. The metalloid group preferably has a hydrocarbyl group, and the hydrocarbyl group of the metalloid group is the same as the hydrocarbyl group described above. Specific examples of the metalloid group include a trimethylsilyl group.

[0068] The central metal M in each general formula is a lanthanoid element, scandium, or yttrium. The lanthanoid element may be any of 15 elements having atomic numbers of 57 to 71. Suitable examples of the central metal M include samarium Sm, neodymium Nd, praseodymium Pr, gadolinium Gd, cerium Ce, holmium Ho, scandium Sc, and yttrium Y.

[0069] The complexes represented by the general formulas (I-1) and (I-2) contain a silylamide ligand [-N(SiR3)2]. The R group (R a ~R f , R g ~R l ) are each independently an alkyl group having 1 to 3 carbon atoms or a hydrogen atom. It is also preferable that at least one of the R groups is a hydrogen atom. By making at least one of the R groups a hydrogen atom, the synthesis of the catalyst becomes easier, and the bulkiness around the silicon becomes lower, making it easier to introduce a non-conjugated olefin compound or an aromatic vinyl compound. From the same viewpoint, in the general formula (I-1), R a ~R c At least one of R is a hydrogen atom. d ~R fIt is more preferable that at least one of R is a hydrogen atom. a ~R c At least one of R is a hydrogen atom. d ~R f At least one of R is a hydrogen atom. g ~R i At least one of R is a hydrogen atom. j ~R l It is more preferable that at least one of the alkyl groups is a hydrogen atom.

[0070] The complexes represented by the general formulae (II-1) and (II-2) contain a silyl ligand [-SiX'3]. X' contained in the silyl ligand [-SiX'3] is a group defined in the same way as X in the general formula (III) described below, and the preferred groups are also the same.

[0071] In general formula (III), X is a group selected from the group consisting of a hydrogen atom, a halogen atom, an alkoxy group, a thiolate group, an amino group, a silyl group, and a monovalent hydrocarbon group having 1 to 20 carbon atoms. Here, the halogen atom represented by X may be any of a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and is preferably a chlorine atom or a bromine atom.

[0072] In the general formula (III), examples of the alkoxy group represented by X include aliphatic alkoxy groups such as methoxy, ethoxy, propoxy, n-butoxy, isobutoxy, sec-butoxy, and tert-butoxy; and aryloxy groups such as phenoxy, 2,6-di-tert-butylphenoxy, 2,6-diisopropylphenoxy, 2,6-dineopentylphenoxy, 2-tert-butyl-6-isopropylphenoxy, 2-tert-butyl-6-neopentylphenoxy, and 2-isopropyl-6-neopentylphenoxy. Of these, 2,6-di-tert-butylphenoxy is preferred.

[0073] In the general formula (III), examples of the thiolate group represented by X include aliphatic thiolate groups such as a thiomethoxy group, a thioethoxy group, a thiopropoxy group, a thio n-butoxy group, a thioisobutoxy group, a thiosec-butoxy group, and a thiotert-butoxy group; and aryl thiolate groups such as a thiophenoxy group, a 2,6-di-tert-butylthiophenoxy group, a 2,6-diisopropylthiophenoxy group, a 2,6-dineopentylthiophenoxy group, a 2-tert-butyl-6-isopropylthiophenoxy group, a 2-tert-butyl-6-thioneopentylphenoxy group, a 2-isopropyl-6-thioneopentylphenoxy group, and a 2,4,6-triisopropylthiophenoxy group. Of these, the 2,4,6-triisopropylthiophenoxy group is preferred.

[0074] In the general formula (III), examples of the amino group represented by X include aliphatic amino groups such as a dimethylamino group, a diethylamino group, and a diisopropylamino group; arylamino groups such as a phenylamino group, a 2,6-di-tert-butylphenylamino group, a 2,6-diisopropylphenylamino group, a 2,6-dineopentylphenylamino group, a 2-tert-butyl-6-isopropylphenylamino group, a 2-tert-butyl-6-neopentylphenylamino group, a 2-isopropyl-6-neopentylphenylamino group, and a 2,4,6-tri-tert-butylphenylamino group; and bistrialkylsilylamino groups such as a bistrimethylsilylamino group. Of these, a bistrimethylsilylamino group is preferred.

[0075] In general formula (III), examples of the silyl group represented by X include a trimethylsilyl group, a tris(trimethylsilyl)silyl group, a bis(trimethylsilyl)methylsilyl group, a trimethylsilyl(dimethyl)silyl group, and a triisopropylsilyl(bistrimethylsilyl)silyl group. Of these, a tris(trimethylsilyl)silyl group is preferred.

[0076] In addition, in general formula (III), specific examples of the monovalent hydrocarbon group having 1 to 20 carbon atoms represented by X include straight-chain or branched-chain aliphatic hydrocarbon groups such as methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, tert-butyl group, neopentyl group, hexyl group, and octyl group; aromatic hydrocarbon groups such as phenyl group, tolyl group, and naphthyl group; aralkyl groups such as benzyl group; and silicon-containing hydrocarbon groups such as trimethylsilylmethyl group and bistrimethylsilylmethyl group. Among these, methyl group, ethyl group, isobutyl group, trimethylsilylmethyl group, and the like are preferred.

[0077] In the general formula (III), X is preferably a bistrimethylsilylamino group or a monovalent hydrocarbon group having 1 to 20 carbon atoms.

[0078] In general formula (III), [B] - Examples of the non-coordinating anion represented by the formula (1) include a tetravalent boron anion. Specific examples of the tetravalent boron anion include tetraphenylborate, tetrakis(monofluorophenyl)borate, tetrakis(difluorophenyl)borate, tetrakis(trifluorophenyl)borate, tetrakis(tetrafluorophenyl)borate, tetrakis(pentafluorophenyl)borate, tetrakis(tetrafluoromethylphenyl)borate, tetra(tolyl)borate, tetra(xylyl)borate, (triphenyl, pentafluorophenyl)borate, [tris(pentafluorophenyl), phenyl]borate, tridecahydride-7,8-dicarbaundecaborate, and the like. Among these, tetrakis(pentafluorophenyl)borate is preferred.

[0079] The complexes represented by the above general formulae (I-1), (I-2), (II-1), (II-2) and (III) further contain 0 to 3, preferably 0 to 1, neutral Lewis bases L. Here, examples of the neutral Lewis base L include tetrahydrofuran, diethyl ether, dimethylaniline, trimethylphosphine, lithium chloride, neutral olefins, and neutral diolefins. Here, when the above complexes contain multiple neutral Lewis bases L, the neutral Lewis bases L may be the same or different.

[0080] In addition, the complexes represented by the above general formulae (I-1), (I-2), (II-1), (II-2) and (III) may exist as a monomer or as a dimer or higher polymer.

[0081] The metallocene complex represented by the above general formula (I-1) can be obtained, for example, by reacting lanthanoid tris halide, scandium tris halide, or yttrium tris halide with an indenyl salt (e.g., potassium salt or lithium salt) and a bis(trialkylsilyl)amine salt (e.g., potassium salt or lithium salt) in a solvent. The reaction temperature may be about room temperature, so that the production can be performed under mild conditions. The reaction time is optional, but is about several hours to several tens of hours. The reaction solvent is not particularly limited, but is preferably a solvent that dissolves the raw materials and the product, and for example, toluene may be used. Below, an example of a reaction for obtaining the metallocene complex represented by the general formula (I-1) is shown. [ka] [In the formula, X″ represents a halide.]

[0082] The metallocene complex represented by the above general formula (II-1) can be obtained, for example, by reacting lanthanoid tris halide, scandium tris halide, or yttrium tris halide with an indenyl salt (e.g., potassium salt or lithium salt) and a silyl salt (e.g., potassium salt or lithium salt) in a solvent. The reaction temperature may be about room temperature, so that the production can be performed under mild conditions. The reaction time is optional, but is about several hours to several tens of hours. The reaction solvent is not particularly limited, but is preferably a solvent that dissolves the raw materials and the product, and for example, toluene may be used. Below, an example of a reaction for obtaining the metallocene complex represented by the general formula (II-1) is shown. [ka] [In the formula, X″ represents a halide.]

[0083] The half metallocene cation complex represented by the above general formula (III) can be obtained, for example, by any of the following reactions. [ka] [ka]

[0084] In the compounds represented by the general formulas (IV-1) and (IV-2), M represents a lanthanoid element, scandium or yttrium, and Cp R’ each independently represents an unsubstituted or substituted cyclopentadienyl, indenyl, or fluorenyl, X represents a hydrogen atom, a halogen atom, an alkoxy group, a thiolate group, an amino group, a silyl group, or a monovalent hydrocarbon group having 1 to 20 carbon atoms, L represents a neutral Lewis base, and w represents an integer of 0 to 3. + [B] - In the ionic compound represented by the formula: [A] + indicates a cation, [B] - indicates a non-coordinating anion.

[0085] [A] + Examples of the cation represented by the formula (I) include carbonium cation, oxonium cation, amine cation, phosphonium cation, cycloheptatrienyl cation, and ferrocenium cation having a transition metal. Examples of the carbonium cation include tri-substituted carbonium cations such as triphenylcarbonium cation and tri(substituted phenyl)carbonium cation, and examples of the tri(substituted phenyl)carbonyl cation include tri(methylphenyl)carbonium cation. Examples of the amine cation include trialkylammonium cations such as trimethylammonium cation, triethylammonium cation, tripropylammonium cation, and tributylammonium cation; N,N-dimethylanilinium cation, N,N-diethylanilinium cation, and N,N-2,4,6-pentamethylanilinium cation; and dialkylammonium cations such as diisopropylammonium cation and dicyclohexylammonium cation. Examples of the phosphonium cation include triarylphosphonium cations such as triphenylphosphonium cation, tri(methylphenyl)phosphonium cation, and tri(dimethylphenyl)phosphonium cation. Among these cations, N,N-dialkylanilinium cations or carbonium cations are preferred, and N,N-dialkylanilinium cations are particularly preferred.

[0086] The general formula [A] used in the above reaction + [B] - The ionic compound represented by the general formula [A] is a compound selected from the above non-coordinating anions and cations and combined, and N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, triphenylcarbonium tetrakis(pentafluorophenyl)borate, etc. are preferred. + [B] -The ionic compound represented by the formula (III) is preferably added in an amount of 0.1 to 10 times by mole, more preferably about 1 times by mole, based on the amount of the metallocene complex. When the half-metallocene cationic complex represented by the formula (III) is used in a polymerization reaction, the half-metallocene cationic complex represented by the formula (III) may be directly provided in the polymerization reaction system, or the compound represented by the formula (IV-1) or (IV-2) used in the reaction and the compound represented by the formula [A] may be directly provided in the polymerization reaction system. + [B] - The ionic compound represented by the general formula (III) may be separately provided in the polymerization reaction system to form a half metallocene cationic complex represented by the general formula (III) in the reaction system. Alternatively, the metallocene complex represented by the general formula (I-1) or (I-2), or the general formula (II-1) or (II-2), and the ionic compound represented by the general formula [A] + [B] - By using the compound represented by the general formula (III) in combination with the ionic compound represented by the general formula (III), a half metallocene cation complex represented by the general formula (III) can be formed in the reaction system.

[0087] The structures of the complexes represented by the above general formulae (I-1), (I-2), (II-1), (II-2) and (III) are preferably determined by X-ray structural analysis.

[0088] The (A-2) component is a rare earth element compound or a reaction product of the rare earth element compound and a Lewis base, and does not have a bond between the rare earth element and carbon. When the rare earth element compound and the reaction product do not have a rare earth element-carbon bond, the compound is stable and easy to handle. Here, the rare earth element compound is a compound containing a rare earth element (M), that is, a lanthanoid element consisting of elements with atomic numbers 57 to 71 in the periodic table, or scandium or yttrium. Specific examples of lanthanoid elements include lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium, and lutetium. The (A-2) component may be used alone or in combination of two or more.

[0089] The rare earth element compound is preferably a salt or complex compound of a divalent or trivalent rare earth metal, and more preferably a rare earth element compound containing one or more ligands selected from hydrogen atoms, halogen atoms, and organic compound residues. Furthermore, the rare earth element compound or the reaction product of the rare earth element compound and a Lewis base is represented by the following general formula (VIII) or (IX): M 11 X 11 2 L 11 w (VIII) M 11 X 11 3·L 11 w (IX) [In each formula, M 11 represents a lanthanide element, scandium or yttrium, and X 11 each independently represents a hydrogen atom, a halogen atom, an alkoxy group, a thiolate group, an amino group, a silyl group, an aldehyde residue, a ketone residue, a carboxylic acid residue, a thiocarboxylic acid residue, or a phosphorus compound residue; L 11 represents a Lewis base, and w represents 0 to 3.

[0090] Examples of the group (ligand) that bonds to the rare earth element of the rare earth element compound include a hydrogen atom, a halogen atom, an alkoxy group (a group obtained by removing hydrogen from a hydroxyl group of an alcohol, which forms a metal alkoxide), a thiolate group (a group obtained by removing hydrogen from a thiol group of a thiol compound, which forms a metal thiolate), an amino group (a group obtained by removing one hydrogen atom bonded to a nitrogen atom of ammonia, a primary amine, or a secondary amine, which forms a metal amide), a silyl group, an aldehyde residue, a ketone residue, a carboxylic acid residue, a thiocarboxylic acid residue, and a phosphorus compound residue. Specific examples of the group (ligand) include a hydrogen atom; an aliphatic alkoxy group such as a methoxy group, an ethoxy group, a propoxy group, an n-butoxy group, an isobutoxy group, a sec-butoxy group, or a tert-butoxy group; a phenoxy group, a 2,6-di-tert-butylphenoxy group, a 2,6-diisopropylphenoxy group, a 2,6-dineopentylphenoxy group, a 2-tert-butyl-6-isopropylphenoxy group, a 2-tert-butyl-6-neopentylphenoxy group, a 2-isopropyl-6-neopentylphenoxy group, aliphatic thiolate groups such as thiomethoxy, thioethoxy, thiopropoxy, thio-n-butoxy, thioisobutoxy, thio-sec-butoxy, and thio-tert-butoxy; thiophenoxy, 2,6-di-tert-butylthiophenoxy, 2,6-diisopropylthiophenoxy, 2,6-dineopentylthiophenoxy, 2-tert-butyl-6-isopropylthiophenoxy, 2-tert-butyl-6-thioneopentylphenoxy, 2-isopropyl-6- Aryl thiolate groups such as thioneopentylphenoxy group and 2,4,6-triisopropylthiophenoxy group; aliphatic amino groups such as dimethylamino group, diethylamino group and diisopropylamino group; phenylamino group, 2,6-di-tert-butylphenylamino group, 2,6-diisopropylphenylamino group, 2,6-dineopentylphenylamino group, 2-tert-butyl-6-isopropylphenylamino group, 2-tert-butyl-6-neopentylphenylamino group, 2-isopropyl arylamino groups such as aryl-6-neopentylphenylamino group and 2,4,6-tri-tert-butylphenylamino group; bistrialkylsilylamino groups such as bistrimethylsilylamino group; silyl groups such as trimethylsilyl group, tris(trimethylsilyl)silyl group, bis(trimethylsilyl)methylsilyl group, trimethylsilyl(dimethyl)silyl group and triisopropylsilyl(bistrimethylsilyl)silyl group; and halogen atoms such as fluorine atom, chlorine atom, bromine atom and iodine atom. Further examples of the group (ligand) include residues of aldehydes such as salicylaldehyde, 2-hydroxy-1-naphthaldehyde, and 2-hydroxy-3-naphthaldehyde; residues of hydroxyphenones such as 2'-hydroxyacetophenone, 2'-hydroxybutyrophenone, and 2'-hydroxypropiophenone; residues of ketones such as acetylacetone, benzoylacetone, propionylacetone, isobutylacetone, valerylacetone, and ethylacetylacetone (particularly residues of diketones). group); residues of carboxylic acids such as isovaleric acid, caprylic acid, octanoic acid, lauric acid, myristic acid, palmitic acid, stearic acid, isostearic acid, oleic acid, linoleic acid, cyclopentanecarboxylic acid, naphthenic acid, ethylhexanoic acid, pivalic acid, Versatic acid [a trade name of Shell Chemical Co., Ltd., a synthetic acid composed of a mixture of isomers of C10 monocarboxylic acids], phenylacetic acid, benzoic acid, 2-naphthoic acid, maleic acid, and succinic acid; hexanethioic acid, 2,2-dimethylbutane Residues of thiocarboxylic acids such as thioacid, decanethioacid, and thiobenzoic acid; dibutyl phosphate, dipentyl phosphate, dihexyl phosphate, diheptyl phosphate, dioctyl phosphate, bis(2-ethylhexyl) phosphate, bis(1-methylheptyl) phosphate, dilauryl phosphate, dioleyl phosphate, diphenyl phosphate, bis(p-nonylphenyl) phosphate, bis(polyethylene glycol-p-nonylphenyl) phosphate, (butyl)(2-ethylhexyl) phosphate, (1-methylheptyl) phosphate )(2-ethylhexyl), phosphate (2-ethylhexyl)(p-nonylphenyl) and other phosphate ester residues; phosphonate ester residues such as monobutyl 2-ethylhexylphosphonate, mono-2-ethylhexyl 2-ethylhexylphosphonate, mono-2-ethylhexyl phenylphosphonate, mono-p-nonylphenyl 2-ethylhexylphosphonate, mono-2-ethylhexyl phosphonate, mono-1-methylheptyl phosphonate, mono-p-nonylphenyl phosphonate and other phosphonate residues;Examples of the phosphinic acid residues include dibutylphosphinic acid, bis(2-ethylhexyl)phosphinic acid, bis(1-methylheptyl)phosphinic acid, dilaurylphosphinic acid, dioleylphosphinic acid, diphenylphosphinic acid, bis(p-nonylphenyl)phosphinic acid, butyl(2-ethylhexyl)phosphinic acid, (2-ethylhexyl)(1-methylheptyl)phosphinic acid, (2-ethylhexyl)(p-nonylphenyl)phosphinic acid, butylphosphinic acid, 2-ethylhexylphosphinic acid, 1-methylheptylphosphinic acid, oleylphosphinic acid, laurylphosphinic acid, phenylphosphinic acid, and p-nonylphenylphosphinic acid. These groups (ligands) may be used alone or in combination of two or more.

[0091] Examples of the Lewis base that reacts with the rare earth element compound include tetrahydrofuran, diethyl ether, dimethylaniline, trimethylphosphine, lithium chloride, neutral olefins, neutral diolefins, etc. Here, when the rare earth element compound reacts with a plurality of Lewis bases (in general formulas (VIII) and (IX), w is 2 or 3), the Lewis base L 11 may be the same or different.

[0092] Preferably, the rare earth element compound is represented by the following general formula (X): M-(AQ 1 )(AQ 2 )(AQ 3 ) (X) [Wherein, M is scandium, yttrium or a lanthanide element; AQ 1 , A.Q. 2 and AQ 3are functional groups which may be the same or different; A is nitrogen, oxygen or sulfur; provided that at least one MA bond is present. Here, the lanthanoid element specifically refers to lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium and lutetium. The compound is a component capable of improving the catalytic activity in the reaction system, shortening the reaction time and increasing the reaction temperature.

[0093] As M in the general formula (X), gadolinium is particularly preferred from the viewpoint of enhancing catalytic activity and reaction controllability.

[0094] When A in the general formula (X) is nitrogen, AQ 1 , A.Q. 2 and AQ 3 (i.e., NQ 1 , NQ 2 and NQ 3 ) is an example of a functional group represented by the formula (I), such as an amino group. In this case, the compound has three M-N bonds.

[0095] Examples of the amino group include aliphatic amino groups such as dimethylamino, diethylamino, and diisopropylamino; arylamino groups such as phenylamino, 2,6-di-tert-butylphenylamino, 2,6-diisopropylphenylamino, 2,6-dineopentylphenylamino, 2-tert-butyl-6-isopropylphenylamino, 2-tert-butyl-6-neopentylphenylamino, 2-isopropyl-6-neopentylphenylamino, and 2,4,6-tri-tert-butylphenylamino; and bistrialkylsilylamino groups such as bistrimethylsilylamino. In particular, from the viewpoint of solubility in aliphatic and aromatic hydrocarbons, bistrimethylsilylamino is preferred. The above amino groups may be used alone or in combination of two or more.

[0096] According to the above-mentioned configuration, the component (A-2) can be a compound having three M-N bonds, and each bond is chemically equivalent, making the compound structure stable and easy to handle. Moreover, the above-mentioned configuration can further improve the catalytic activity in the reaction system, thereby enabling the reaction time to be further shortened and the reaction temperature to be further increased.

[0097] When A in the general formula (X) is oxygen, the general formula (X) (i.e., M-(OQ 1 )(OQ 2 )(OQ 3 The rare earth element-containing compound represented by the formula (XI) is not particularly limited, but may be, for example, a compound represented by the formula (XI): (RO)3M ··· (XI) and rare earth alcoholates represented by the following general formula (XII): (R-CO2)3M (XII) and rare earth carboxylates represented by the following formula: In the above general formulas (XI) and (XII), R may be the same or different and is an alkyl group having 1 to 10 carbon atoms.

[0098] When A in the general formula (X) is sulfur, the general formula (X) (i.e., M-(SQ 1 )(SQ 2 )(SQ 3 The rare earth element-containing compound represented by the formula (XIII) is not particularly limited, but may be, for example, a compound represented by the formula (XIII): (RS)3M (XIII) and rare earth alkylthiolates represented by the following general formula (XIV): (R-CS2)3M (XIV) and the like. In the above general formulas (XIII) and (XIV), R may be the same or different and is an alkyl group having 1 to 10 carbon atoms.

[0099] The organometallic compound (component (B)) is represented by the following general formula (XV): YR1 a R 2 b R 3 c (XV) [In the formula, Y is a metal selected from Groups 1, 2, 12, and 13 of the periodic table; R 1 and R 2 is a hydrocarbon group having 1 to 10 carbon atoms or a hydrogen atom, R 3 is a hydrocarbon group having 1 to 10 carbon atoms, where R 1 , R 2 and R 3 may be the same or different, and when Y is a metal selected from Group 1 of the periodic table, a is 1 and b and c are 0; when Y is a metal selected from Groups 2 and 12 of the periodic table, a and b are 1 and c is 0; and when Y is a metal selected from Group 13 of the periodic table, a, b, and c are 1.

[0100] In the above general formula (XV), R 1 , R 2 and R 3 Specific examples of the hydrocarbon group having 1 to 10 carbon atoms represented by the formula (I) include straight-chain or branched-chain aliphatic hydrocarbon groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, neopentyl, hexyl, and octyl; aromatic hydrocarbon groups such as phenyl, tolyl, and naphthyl; and aralkyl groups such as benzyl. Of these, methyl, ethyl, and isobutyl groups are preferred.

[0101] The component (B) is preferably a compound represented by the following general formula (XVI): AlR 1 R 2 R 3 (XVI) [In the formula, R 1 and R 2 is a hydrocarbon group having 1 to 10 carbon atoms or a hydrogen atom, R 3 is a hydrocarbon group having 1 to 10 carbon atoms, where R 1 , R 2 and R3 and may be the same or different from each other. The organoaluminum compound corresponds to the compound represented by the above general formula (XV) in which Y is Al, and a, b, and c are 1.

[0102] Examples of the organoaluminum compound of the general formula (XVI) include trimethylaluminum, triethylaluminum, tri-n-propylaluminum, triisopropylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-t-butylaluminum, tripentylaluminum, trihexylaluminum, tricyclohexylaluminum, trioctylaluminum; diethylaluminum hydride, di-n-propylaluminum hydride, di-n-butylaluminum hydride, diisobutylaluminum hydride, dihexylaluminum hydride, diisohexylaluminum hydride, dioctylaluminum hydride, diisooctylaluminum hydride; ethylaluminum dihydride, n-propylaluminum dihydride, isobutylaluminum dihydride, and the like. Among these, triethylaluminum, triisobutylaluminum, diethylaluminum hydride, and diisobutylaluminum hydride are preferred.

[0103] The (B) component may be used alone or in combination of two or more. When the (B) component is used together with the above-mentioned (A) component, the amount of the (B) component used is preferably 1 to 50 times by mol, more preferably about 10 times by mol, relative to the amount of the (A) component.

[0104] The aluminoxane (component (C)) is a compound obtained by contacting an organoaluminum compound with a condensing agent. By using component (C), the catalytic activity in the polymerization reaction system can be further improved, so that the desired copolymer can be easily obtained. In addition, the reaction time can be further shortened and the reaction temperature can be further increased.

[0105] Examples of the organoaluminum compound include trialkylaluminum such as trimethylaluminum, triethylaluminum, and triisobutylaluminum, and mixtures thereof. In particular, trimethylaluminum and a mixture of trimethylaluminum and tributylaluminum are preferred. On the other hand, the condensing agent may, for example, be water.

[0106] Examples of the component (C) include compounds represented by the following formula (XVII): -(Al(R 7 )O) n - (XVII) [In the formula, R 7 is a hydrocarbon group having 1 to 10 carbon atoms, a part of which may be substituted with a halogen and / or an alkoxy group; R 7 may be the same or different between the repeating units; and n is 5 or more. The molecular structure of the aluminoxane may be linear or cyclic. In the above formula (XVII), n is preferably 10 or more. In addition, R in the above formula (XVII) 7 With respect to the above, examples of the hydrocarbon group include a methyl group, an ethyl group, a propyl group, an isobutyl group, and the like, and a methyl group is particularly preferred. The hydrocarbon group may be one type or a combination of two or more types. 7 Regarding the above, the hydrocarbon group is preferably a combination of a methyl group and an isobutyl group. The aluminoxane preferably has high solubility in aliphatic hydrocarbons and low solubility in aromatic hydrocarbons, for example, aluminoxanes commercially available as a hexane solution are preferred. Examples of the aliphatic hydrocarbon include hexane and cyclohexane.

[0107] The component (C) is particularly represented by the following formula (XVIII): -(Al(CH3) x (i-C4H9) y O) m - (XVIII) [wherein x+y is 1; m is 5 or more]. An example of TMAO is a product named "TMAO-341" manufactured by Tosoh Fine Chemicals Corporation.

[0108] The component (C) is particularly a compound represented by the following formula (XIX): -(Al(CH3) 0.7 (i-C4H9) 0.3 O) k - (XIX) In the formula, k is 5 or more. An example of the MMAO is a product named "MMAO-3A" manufactured by Tosoh Fine Chemicals Corporation.

[0109] Furthermore, the component (C) is particularly a compound represented by the following formula (XX): -[(CH3)AlO] i - (XX) In the formula, i is 5 or more. An example of PMAO is PMAO-211, a product of Tosoh Fine Chemicals Corporation.

[0110] From the viewpoint of enhancing the effect of improving the catalytic activity, the component (C) is preferably MMAO or TMAO among the above-mentioned MMAO, TMAO, and PMAO, and in particular, from the viewpoint of further enhancing the effect of improving the catalytic activity, it is more preferably TMAO.

[0111] The (C) component may be used alone or in combination of two or more. From the viewpoint of improving catalytic activity, when the (C) component is used together with the (A) component, the (C) component is preferably used in such an amount that the amount of aluminum in the (C) component is 10 mol or more, more preferably 100 mol or more, and more preferably 1000 mol or less, more preferably 800 mol or less, per mol of rare earth element in the (A) component.

[0112] The ionic compound (component (D)) comprises a non-coordinating anion and a cation. When the component (D) is used together with the above-mentioned component (A), the component (D) may be an ionic compound capable of reacting with the component (A) to produce a cationic transition metal compound.

[0113] Here, examples of the non-coordinating anion include tetravalent boron anions, such as tetraphenylborate, tetrakis(monofluorophenyl)borate, tetrakis(difluorophenyl)borate, tetrakis(trifluorophenyl)borate, tetrakis(tetrafluorophenyl)borate, tetrakis(pentafluorophenyl)borate, tetrakis(tetrafluoromethylphenyl)borate, tetra(tolyl)borate, tetra(xylyl)borate, (triphenyl, pentafluorophenyl)borate, [tris(pentafluorophenyl), phenyl]borate, and tridecahydride-7,8-dicarbaundecaborate. Among these, tetrakis(pentafluorophenyl)borate is preferred.

[0114] On the other hand, examples of the cation include carbonium cation, oxonium cation, amine cation, phosphonium cation, cycloheptatrienyl cation, ferrocenium cation having a transition metal, etc. Specific examples of the carbonium cation include tri-substituted carbonium cations such as triphenylcarbonium cation (also called "trityl cation") and tri(substituted phenyl)carbonium cation, etc. More specifically, examples of the tri(substituted phenyl)carbonyl cation include tri(methylphenyl)carbonium cation and tri(dimethylphenyl)carbonium cation. Examples of the amine cation include ammonium cations, and specific examples of the ammonium cation include trialkylammonium cations such as trimethylammonium cation, triethylammonium cation, tripropylammonium cation, and tributylammonium cation (e.g., tri(n-butyl)ammonium cation); N,N-dialkylanilinium cations such as N,N-dimethylanilinium cation, N,N-diethylanilinium cation, and N,N-2,4,6-pentamethylanilinium cation; and dialkylammonium cations such as diisopropylammonium cation and dicyclohexylammonium cation. Specific examples of the phosphonium cation include triarylphosphonium cations such as triphenylphosphonium cation, tri(methylphenyl)phosphonium cation, and tri(dimethylphenyl)phosphonium cation. Among these cations, N,N-dialkylanilinium cation or carbonium cation is preferred, and N,N-dialkylanilinium cation is particularly preferred.

[0115] Therefore, the ionic compound (component (D)) is preferably a compound in which the non-coordinating anions and cations are selected and combined from the above-mentioned non-coordinating anions and cations. Specifically, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, triphenylcarbonium tetrakis(pentafluorophenyl)borate, etc. are preferred.

[0116] The (D) component may be used alone or in combination of two or more. When the (D) component is used together with the (A) component, the amount of the (D) component used is preferably 0.1 to 10 times by mol, more preferably about 1 times by mol, relative to the (A) component.

[0117] Examples of the halogen compound (component (E)) include a halogen-containing compound that is a Lewis acid (hereinafter also referred to as "component (E-1)"), a complex compound of a metal halide and a Lewis base (hereinafter also referred to as "component (E-2)"), and an organic compound containing an active halogen (hereinafter also referred to as "component (E-3)"). When the component (E) is used together with the above-mentioned component (A), for example, it can react with the component (A) to produce a cationic transition metal compound, a transition metal halide compound, or a compound in which the transition metal center is undercharged.

[0118] As the (E-1) component, for example, a halogen compound containing an element of group 3, 4, 5, 6, 8, 13, 14 or 15 in the periodic table can be used. Aluminum halides or organometallic halides are preferable. Moreover, the halogen element is preferably chlorine or bromine. Specific examples of the halogen-containing compound that is the Lewis acid include methylaluminum dibromide, methylaluminum dichloride, ethylaluminum dibromide, ethylaluminum dichloride, butylaluminum dibromide, butylaluminum dichloride, dimethylaluminum bromide, dimethylaluminum chloride, diethylaluminum bromide, diethylaluminum chloride, dibutylaluminum bromide, dibutylaluminum chloride, methylaluminum sesquibromide, methylaluminum sesquichloride, ethylaluminum sesquibromide, ethylaluminum sesquichloride, dibutyltin dichloride, aluminum tribromide, tri(pentafluorophenyl)aluminum, tri(pentafluorophenyl)borate, antimony trichloride, antimony pentachloride, phosphorus trichloride, phosphorus pentachloride, tin tetrachloride, titanium tetrachloride, and tungsten hexachloride. Among these, diethylaluminum chloride, ethylaluminum sesquichloride, ethylaluminum dichloride, diethylaluminum bromide, ethylaluminum sesquibromide, and ethylaluminum dibromide are particularly preferred. The component (E-1) may be used alone or in combination of two or more.

[0119] Examples of metal halides constituting the above component (E-2) include beryllium chloride, beryllium bromide, beryllium iodide, magnesium chloride, magnesium bromide, magnesium iodide, calcium chloride, calcium bromide, calcium iodide, barium chloride, barium bromide, barium iodide, zinc chloride, zinc bromide, zinc iodide, cadmium chloride, cadmium bromide, cadmium iodide, mercury chloride, mercury bromide, mercury iodide, manganese chloride, manganese bromide, manganese iodide, rhenium chloride, rhenium bromide, rhenium iodide, copper chloride, copper iodide, silver chloride, silver bromide, silver iodide, gold chloride, gold iodide, gold bromide, and the like. Among these, magnesium chloride, calcium chloride, barium chloride, manganese chloride, zinc chloride, and copper chloride are preferred, and magnesium chloride, manganese chloride, zinc chloride, and copper chloride are particularly preferred. In addition, the Lewis base constituting the component (E-2) is preferably a phosphorus compound, a carbonyl compound, a nitrogen compound, an ether compound, an alcohol, etc. Specifically, tributyl phosphate, tri-2-ethylhexyl phosphate, triphenyl phosphate, tricresyl phosphate, triethylphosphine, tributylphosphine, triphenylphosphine, diethylphosphinoethane, diphenylphosphinoethane, acetylacetone, benzoylacetone, propionitrileacetone, valerylacetone, ethylacetylacetone, methyl acetoacetate, ethyl acetoacetate, phenyl acetoacetate, dimethyl malonate, diethyl malonate, diphenyl malonate, acetic acid, octanoic acid, 2-ethyl-hexanoic acid, oleic acid, etc. , stearic acid, benzoic acid, naphthenic acid, Versatic acid, triethylamine, N,N-dimethylacetamide, tetrahydrofuran, diphenyl ether, 2-ethyl-hexyl alcohol, oleyl alcohol, stearyl alcohol, phenol, benzyl alcohol, 1-decanol, lauryl alcohol, etc., and among these, tri-2-ethylhexyl phosphate, tricresyl phosphate, acetylacetone, 2-ethylhexanoic acid, Versatic acid, 2-ethylhexyl alcohol, 1-decanol, and lauryl alcohol are preferred. The Lewis base is reacted in an amount of 0.01 to 30 mol, preferably 0.5 to 10 mol, per mol of the metal halide. By using the reaction product with the Lewis base, the amount of metal remaining in the polymer can be reduced. The above component (E-2) may use one type alone, or two or more types in combination.

[0120] Examples of the component (E-3) include benzyl chloride.

[0121] The component (E) may be used alone or in combination of two or more. When the component (E) is used together with the component (A), the amount of the component (E) used is preferably 0 to 5 times, more preferably 1 to 5 times, the amount of the component (A).

[0122] The cyclopentadiene skeleton-containing compound (component (F)) has a group selected from a cyclopentadienyl group, an indenyl group, and a fluorenyl group, and the cyclopentadiene skeleton-containing compound (F) is at least one compound selected from the group consisting of substituted or unsubstituted cyclopentadiene, substituted or unsubstituted indene, and substituted or unsubstituted fluorene. The component (F) may be used alone or in combination of two or more.

[0123] Examples of the substituted or unsubstituted cyclopentadiene include cyclopentadiene, pentamethylcyclopentadiene, tetramethylcyclopentadiene, isopropylcyclopentadiene, trimethylsilyl-tetramethylcyclopentadiene, and (1-benzyldimethylsilyl)cyclopenta[l]phenanthrene.

[0124] Examples of the substituted or unsubstituted indenes include indene, 2-phenyl-1H-indene, 3-benzyl-1H-indene, 3-methyl-2-phenyl-1H-indene, 3-benzyl-2-phenyl-1H-indene, 1-benzyl-1H-indene, 1-methyl-3-dimethylbenzylsilyl-indene, 1,3-bis(t-butyldimethylsilyl)-indene, (1-benzyldimethylsilyl-3-cyclopentyl)indene, (1-benzyl-3-t-butyldimethylsilyl)indene, and the like. In particular, from the viewpoint of narrowing the molecular weight distribution, 3-benzyl-1H-indene and 1-benzyl-1H-indene are preferred.

[0125] Examples of the substituted or unsubstituted fluorene include fluorene, trimethylsilylfluorene, and isopropylfluorene.

[0126] In particular, the cyclopentadiene skeleton-containing compound (component (F)) is preferably a substituted cyclopentadiene, a substituted indene, or a substituted fluorene, and more preferably a substituted indene. This advantageously increases the bulkiness of the polymerization catalyst, allowing the reaction time to be shortened and the reaction temperature to be increased. In addition, since the compound has many conjugated electrons, the catalytic activity in the reaction system can be further improved.

[0127] Here, examples of the substituent of the substituted cyclopentadiene, substituted indene, and substituted fluorene include hydrocarbyl groups and metalloid groups, and the number of carbon atoms in the hydrocarbyl group is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 8. Specific examples of the hydrocarbyl group include methyl groups, ethyl groups, phenyl groups, and benzyl groups. On the other hand, examples of the metalloid of the metalloid group include germyl Ge, stannyl Sn, and silyl Si, and the metalloid group preferably has a hydrocarbyl group, and the hydrocarbyl group of the metalloid group is the same as the hydrocarbyl group described above. Specific examples of the metalloid group include trimethylsilyl groups.

[0128] The (F) component may be used alone or in combination of two or more. In addition, from the viewpoint of improving catalytic activity, when the (F) component is used together with the (A) component, the molar ratio of the (F) component to the (A) component is preferably more than 0, more preferably 0.5 or more, and particularly preferably 1 or more, and is preferably 3 or less, more preferably 2.5 or less, and particularly preferably 2.2 or less.

[0129] The above-mentioned components (A) to (F) are preferably used in various combinations as catalyst compositions in the polymerization step. Suitable catalyst compositions include the following first and second catalyst compositions. Note that the first and second catalyst compositions have not been used in the polymerization (synthesis of binary copolymers) of at least conjugated diene compounds and non-conjugated olefin compounds.

[0130] The first catalyst composition contains the (A-1) component, the (B) component, and the (D) component, and further contains at least one of the (C) component and the (E) component as optional components. Note that when the (A-1) component is a metallocene-based composite catalyst represented by the general formula (V), the (B) component is also an optional component.

[0131] The second catalyst composition contains the (A-2) component, the (B) component, and the (D) component, and further contains at least one of the (C), (E) and (F) components as optional components. When the second catalyst composition contains the (F) component, the catalytic activity is improved.

[0132] The coupling step is a step of carrying out a reaction (coupling reaction) for modifying at least a part (for example, an end) of the polymer chain of the copolymer obtained in the polymerization step. In the coupling step, it is preferable to carry out the coupling reaction when the polymerization reaction reaches 100%. The coupling agent used in the coupling reaction is not particularly limited and can be appropriately selected depending on the purpose, and examples thereof include tin-containing compounds such as bis(1-octadecylmaleate)dioctyltin(IV), isocyanate compounds such as 4,4'-diphenylmethane diisocyanate, alkoxysilane compounds such as glycidylpropyltrimethoxysilane, etc. These may be used alone or in combination of two or more. Among these, bis(1-octadecylmaleate)dioctyltin(IV) is preferred in terms of reaction efficiency and low gel formation. By carrying out a coupling reaction, the number average molecular weight (Mn) can be increased.

[0133] The washing step is a step of washing the copolymer obtained in the polymerization step. The medium used for washing is not particularly limited and can be appropriately selected according to the purpose, and examples thereof include methanol, ethanol, and isopropanol. When a catalyst derived from a Lewis acid is used as a polymerization catalyst, an acid (e.g., hydrochloric acid, sulfuric acid, nitric acid, etc.) can be added to these solvents. The amount of acid added is preferably 15 mol% or less relative to the solvent. If the amount is more than this, the acid may remain in the copolymer, which may adversely affect the reaction during kneading and vulcanization. This washing step makes it possible to suitably reduce the amount of catalyst residue in the copolymer.

[0134] The copolymer of the present embodiment, which has a characteristic curve (DSC curve) obtained by a differential scanning calorimeter, can be preferably obtained by preparing a solution of a conjugated diene compound in a reactor, then adding a catalyst component or catalyst composition to the reactor and heating it to a predetermined temperature, and then continuously adding the solution of the conjugated diene compound to the reactor while introducing a non-conjugated olefin compound at a predetermined pressure.

[0135] The adjustment method for obtaining the above copolymer includes, for example, (1) making the addition rate of the conjugated diene compound relatively slow (performing polymerization over a relatively long period of time), (2) using a relatively large amount of the non-conjugated olefin compound, or (3) making the amount of at least one of the above components (B) and (D) relatively small. In this regard, the main factor for controlling the length of the chain derived from the non-conjugated olefin compound is the concentration of the conjugated diene compound. Therefore, among the above, (1) and (2), especially (1) are considered to be more important.

[0136] (Rubber composition) A rubber composition according to one embodiment of the present invention (hereinafter, sometimes referred to as "rubber composition of the present embodiment") is characterized by containing the copolymer described above. Since the rubber composition of the present embodiment contains the copolymer described above, it has excellent cut resistance and ozone resistance.

[0137] The rubber composition of the present embodiment contains the above-mentioned copolymer as a rubber component, and may further contain other rubber components as necessary.

[0138] The other rubber components are not particularly limited and can be appropriately selected according to the purpose. For example, natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber (NBR), chloroprene rubber, ethylene-propylene rubber (EPM), ethylene-propylene-diene rubber (EPDM), polysulfide rubber, silicone rubber, fluororubber, urethane rubber, etc. may be mentioned. These rubber components may be used alone or in combination of two or more. In particular, natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), and styrene-butadiene rubber (SBR) are preferable as the other rubber components.

[0139] In the rubber composition of the present embodiment, the proportion of the copolymer in the rubber component is preferably 10% by mass or more. If the proportion of the copolymer in the rubber component is 10% by mass or more, the effect of the copolymer is fully exerted, and the cut resistance and ozone resistance of the rubber composition can be sufficiently improved. From the same viewpoint, the proportion of the copolymer in the rubber component is more preferably 30% by mass or more, further preferably 50% by mass or more, and can also be 100% by mass.

[0140] The rubber composition of the present embodiment may further contain a filler, a crosslinking agent, an antioxidant, and the like as appropriate.

[0141] Examples of the filler include carbon black, silica, aluminum hydroxide, clay, alumina, talc, mica, kaolin, glass balloons, glass beads, calcium carbonate, magnesium carbonate, magnesium hydroxide, magnesium oxide, titanium oxide, potassium titanate, barium sulfate, etc. These fillers may be used alone or in combination of two or more. Among these, carbon black and silica are preferred as the filler.

[0142] The content of the filler in the rubber composition of the present embodiment is preferably 10 parts by mass or more and 100 parts by mass or less per 100 parts by mass of the rubber component. When the content of the filler is 10 parts by mass or more, the effect of improving the reinforcing property by compounding the filler can be obtained, and when the content is 100 parts by mass or less, good workability can be maintained. From the same viewpoint, the content of the filler in the rubber composition is more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, and more preferably 80 parts by mass or less, and even more preferably 60 parts by mass or less per 100 parts by mass of the rubber component.

[0143] Examples of the crosslinking agent include sulfur-based crosslinking agents such as sulfur, organic peroxide-based crosslinking agents, inorganic crosslinking agents, polyamine crosslinking agents, resin crosslinking agents, oxime-nitrosamine crosslinking agents, etc. Among these, the crosslinking agent is preferably a sulfur-based crosslinking agent (vulcanizing agent), and more preferably sulfur.

[0144] The content of the crosslinking agent in the rubber composition of the present embodiment is preferably 0.1 to 20 parts by mass based on 100 parts by mass of the rubber component.

[0145] When the vulcanizing agent is used, the rubber composition of the present embodiment may further contain a vulcanization accelerator. Examples of the vulcanization accelerator include guanidine-based, aldehyde-amine-based, aldehyde-ammonia-based, thiazole-based, sulfenamide-based, thiourea-based, thiuram-based, dithiocarbamate-based, and xanthate-based compounds.

[0146] Examples of the antiaging agent include amine-ketone compounds, imidazole compounds, amine compounds, phenol compounds, sulfur compounds, and phosphorus compounds. In particular, the rubber composition of the present embodiment preferably contains a compound having two or more phenyl groups with a branched alkyl group as the antiaging agent. In this way, by using a compound having two or more phenyl groups with a branched alkyl group as the antiaging agent, the dispersibility of the copolymer of the present embodiment can be improved and the gelation of the copolymer of the present embodiment can be suppressed. The compound having two or more phenyl groups with a branched alkyl group may be used alone or in combination of two or more.

[0147] More specifically, the compound having two or more phenyl groups having a branched alkyl group is preferably a compound having a structure represented by the following formula (1) or formula (2).

[0148] [ka]

[0149] [ka]

[0150] In the above formula (1) and formula (2), R 1 ~R 8 , R 11 ~R 18 , and R 21 ~R 24 is a hydrogen atom, a linear alkyl group, a cyclic alkyl group, or a branched alkyl group, and R 1 ~R 8 At least one of; and R 11 ~R 18 and R 21 ~R 24 At least one of R is a branched alkyl group. 1 ~R 8 , R 11 ~R 18 , and R21 ~R 24 may be the same or different. 9 is a hydrocarbon group. 1 and A 2 is a linking group. E is a trivalent heteroatom.

[0151] The number of carbon atoms in the linear alkyl group is preferably 1 to 12, more preferably 1 to 8, even more preferably 1 to 5, and even more preferably 1 to 3. Specific examples of the linear alkyl group include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, an n-decyl group, and an n-dodecyl group. The linear alkyl group may further have a substituent such as a halogen atom. Of the above, the straight-chain alkyl group is preferably an unsubstituted straight-chain alkyl group, and more preferably a methyl group, an ethyl group, or an n-propyl group.

[0152] The number of carbon atoms in the cyclic alkyl group is preferably 5 to 12, more preferably 6 to 12, and even more preferably 6 to 8. Specific examples of the cyclic alkyl group include a cyclopentyl group, a cyclohexyl group, and a cyclooctyl group. The cyclic alkyl group may further have a substituent such as an alkyl group having 1 to 3 carbon atoms or a halogen atom. Of the above, the cyclic alkyl group is preferably an unsubstituted cyclic alkyl group, and more preferably a cyclohexyl group.

[0153] The number of carbon atoms in the branched alkyl group is preferably 3 to 12, more preferably 3 to 8, even more preferably 4 to 8, and even more preferably 4 to 6. Specific examples of the branched alkyl group include an isopropyl group, a 2-butyl group, a tert-butyl group, a tert-pentyl group, a 2-hexyl group, a 2-heptyl group, a 2-octyl group, and a 2-dodecyl group. The branched alkyl group may further have a substituent such as a halogen atom. Among the above, the branched alkyl group is preferably an unsubstituted branched alkyl group, more preferably an isopropyl group, a 2-butyl group, a tert-butyl group, or a tert-pentyl group, and even more preferably a tert-butyl group or a tert-pentyl group.

[0154] R 9 Examples of the hydrocarbon group represented by the formula (1) include an alkyl group, an alkenyl group, and an alkynyl group. Examples of the alkyl group include the linear alkyl group, cyclic alkyl group, and branched alkyl group exemplified above, and the preferred ranges are the same. In addition, the alkenyl group and the alkynyl group are preferably those having 2 to 8 carbon atoms, and examples thereof include a vinyl group.

[0155] A 1 and A 2 Examples of the linking group represented by the formula (I) include a divalent hydrocarbon group having 1 to 6 carbon atoms, and may contain a heteroatom having a valence of 2 or more (for example, an oxygen atom, a sulfur atom, etc.). The hydrocarbon of the hydrocarbon group may be a saturated hydrocarbon or an unsaturated hydrocarbon. Of these, the linking group is preferably a saturated hydrocarbon group, and the number of carbon atoms of the linking group is preferably 1 to 5, and more preferably 1 to 4. The linking group may further have a substituent such as a halogen atom, a methyl group, or an ethyl group.

[0156] Examples of the trivalent heteroatom represented by E include a sulfur atom and a phosphorus atom, and among these, a phosphorus atom is preferable.

[0157] In formula (1), R 1 ~R 4 At least one of, and R 5 ~R 8 In addition, in the formula (2), at least one of R 11 ~R 14 a group Ra selected from the group 15 ~R 18 A group Rb selected from the group consisting of: 21 ~R24 It is preferred that at least two selected from the group consisting of groups Rc selected from the group consisting of: are branched alkyl groups.

[0158] Furthermore, it is preferable that the phenyl group having a branched alkyl group (phenyl group with branched alkyl groups) has a plurality of branched alkyl groups. 1 ~R 4 At least two of R 5 ~R 8 At least two of R 11 ~R 14 At least two of; and R 15 ~R 18 It is preferred that at least two of the groups are branched alkyl groups.

[0159] The compound having the structure represented by formula (1) is preferably as follows: R 1 and R 8 is a branched alkyl group; R 2 , R 4 , R 5 and R 7 is a hydrogen atom; R 3 and R 6 is a branched or linear alkyl group; R 9 is an unsaturated hydrocarbon group; A 1 is a divalent saturated hydrocarbon group.

[0160] More preferably, the compound having the structure represented by formula (1) is as follows: R 1 and R 8 is an unsubstituted branched alkyl group having 3 to 6 carbon atoms; R 2 , R 4 , R 5 and R 7 is a hydrogen atom; R 3 and R 6 is an unsubstituted branched alkyl group having 4 to 5 carbon atoms or an unsubstituted linear alkyl group having 1 to 3 carbon atoms; R 9 A is an unsubstituted vinyl group; 1 is an unsubstituted or substituted methylene group.

[0161] The compound having the structure represented by formula (1) is more preferably a compound having a structure represented by the following formula (3) or (4).

[0162] [ka]

[0163] [ka]

[0164] The structure represented by formula (2) is preferably as follows: R 11 , R 13 , R 16 , R 18 and R 21 is a branched alkyl group; R 12 , R 14 , R 15 , R 17 , R 22 and R 23 is a hydrogen atom; R 24 is a straight chain alkyl group; A 2 is a divalent saturated hydrocarbon group containing an oxygen atom; E is a sulfur atom or a phosphorus atom.

[0165] Moreover, the structure represented by formula (2) is more preferably as follows: R 11 , R 13 , R 16 , R 18 and R 21 is an unsubstituted branched alkyl group having 3 to 5 carbon atoms; R 12 , R 14 , R 15 , R 17 , R 22 and R 23 is a hydrogen atom; R 24 is an unsubstituted linear alkyl group having 1 to 3 carbon atoms; A 2is an unsubstituted alkyleneoxy group having 2 to 5 carbon atoms (in -OR-, R is an unsubstituted alkylene having 2 to 5 carbon atoms); E is a phosphorus atom.

[0166] The compound having the structure represented by formula (2) is more preferably a compound having a structure represented by the following formula (5).

[0167] [ka]

[0168] Among the above, the compound having two or more phenyl groups each having a branched alkyl group is particularly preferably a compound having a structure represented by the above formula (4) or formula (5).

[0169] The content of the antiaging agent in the rubber composition of the present embodiment is preferably 0.1 parts by mass or more and 5 parts by mass or less per 100 parts by mass of the copolymer. If the content of the antiaging agent is 0.1 parts by mass or more, the effect of improving the dispersibility of the copolymer and suppressing gelation can be sufficiently obtained, and if it is 5 parts by mass or less, the cut resistance can be well maintained. From the same viewpoint, the content of the antiaging agent in the rubber composition is more preferably 0.5 parts by mass or more, and more preferably 3 parts by mass or less.

[0170] In addition to the above, the rubber composition of the present embodiment may contain, as necessary, appropriate amounts of known additives such as softeners, vulcanization aids, colorants, flame retardants, lubricants, foaming agents, plasticizers, processing aids, antioxidants, scorch inhibitors, ultraviolet inhibitors, antistatic agents, color inhibitors, and other compounding agents depending on the intended use.

[0171] The rubber composition of the present embodiment can be suitably used for rubber products such as tires, anti-vibration rubber, seismic isolation rubber, belts such as conveyor belts, rubber crawlers, and various hoses.

[0172] (Resin composition) The resin composition according to one embodiment of the present invention (hereinafter, sometimes referred to as "the resin composition of the present embodiment") is characterized by containing the copolymer described above. Since the resin composition of the present embodiment contains the copolymer described above, it has excellent cut resistance and ozone resistance.

[0173] The resin composition of the present embodiment contains the above-mentioned copolymer as a resin component, and may further contain other resin components as necessary. Note that, with respect to the resin composition of the present embodiment, the copolymer is treated as the resin component.

[0174] The other resin components are not particularly limited and can be appropriately selected depending on the purpose. Examples of the other resin components include thermoplastic resins such as polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyamide, polycarbonate, polyoxymethylene, and polyphenylene ether, and thermosetting resins such as phenol resins, epoxy resins, urea resins, and melamine resins.

[0175] In the resin composition of the present embodiment, the proportion of the copolymer in the resin component is preferably 10% by mass or more. If the proportion of the copolymer in the resin component is 10% by mass or more, the effect of the copolymer is fully exerted, and the cut resistance and ozone resistance of the resin composition can be fully improved. From the same viewpoint, the proportion of the copolymer in the resin component is more preferably 30% by mass or more, further preferably 50% by mass or more, and can also be 100% by mass.

[0176] The resin composition of the present embodiment may further contain various additives as appropriate, such as an antistatic agent, a lubricant, a crystal nucleating agent, a tackifier, an antifogging agent, a release agent, a plasticizer, a filler, an antioxidant, an antiaging agent, a pigment, a dye, a fragrance, and a flame retardant.

[0177] In particular, the antiaging agent may be a compound having two or more branched alkyl group-bearing phenyl groups as described above, and the resin composition of the present embodiment preferably contains such a compound having two or more branched alkyl group-bearing phenyl groups. In this way, by using a compound having two or more branched alkyl group-bearing phenyl groups as an antiaging agent, the dispersibility of the copolymer of the present embodiment can be improved and the gelation of the copolymer of the present embodiment can be suppressed. The above-mentioned compound having two or more branched alkyl group-bearing phenyl groups may be used alone or in combination of two or more.

[0178] The preferred structure of the compound having two or more branched alkyl group-containing phenyl groups and the content thereof in the resin composition are the same as those described above regarding the rubber composition.

[0179] The resin composition of the present embodiment can be suitably used, for example, in various resin products having at least a resin portion in a part thereof. EXAMPLES

[0180] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0181] Example 1: Preparation of Copolymer A 20 g of a toluene solution containing 5 g of 1,3-butadiene and 480 g of toluene were added to a thoroughly dried 2000 mL pressure-resistant stainless steel reactor. Ethylene was then added to the pressure-resistant stainless steel reactor at a pressure of about 1.0 MPa, and the system was replaced with ethylene three times. Meanwhile, in a glove box under a nitrogen atmosphere, 0.025 mmol of mono(bis(1,3-tert-butyldimethylsilyl)indenyl)bis(bis(dimethylsilyl)amide) gadolinium complex {1,3-[(t-Bu)Me2Si]2C9H5Gd[N(SiHMe2)2]2}, 0.025 mmol of trityl tetrakis(pentafluorophenyl)borate [Ph3CB(C6F5)4], and 0.75 mmol of triisobutylaluminum were charged into a glass vessel, and 15 mL of toluene was added to obtain a catalyst solution. After aging for 1 hour, the catalyst solution was added to the pressure-resistant stainless steel reactor and heated to 80°C. Next, ethylene was charged into the pressure-resistant stainless steel reactor at a pressure of 1.0 MPa, and copolymerization was carried out at 80° C. while further adding 100 g of a toluene solution containing 25 g of 1,3-butadiene over a period of 60 minutes. Next, 1 mL of a 5% by mass solution of 2,2'-methylene-bis(4-ethyl-6-t-butylphenol) (NS-5) in isopropanol was added to the pressure-resistant stainless steel reactor to terminate the reaction. Next, separation was carried out using a large amount of methanol and vacuum drying at 50° C. to obtain copolymer A.

[0182] Example 2: Preparation of Copolymer B A 2000 mL pressure-resistant stainless steel reactor that had been thoroughly dried was charged with 40 g of a toluene solution containing 10 g of 1,3-butadiene and 460 g of toluene. Ethylene was then added to the reactor at a pressure of about 1.0 MPa, and the system was replaced with ethylene three times. Meanwhile, in a glove box under a nitrogen atmosphere, 0.075 mmol of mono(bis(1,3-tert-butyldimethylsilyl)indenyl)bis(bis(dimethylsilyl)amide) gadolinium complex {1,3-[(t-Bu)Me2Si]2C9H5Gd[N(SiHMe2)2]2}, 0.025 mmol of trityl tetrakis(pentafluorophenyl)borate [Ph3CB(C6F5)4], and 0.25 mmol of triisobutylaluminum were charged into a glass vessel, and 10 mL of toluene was added to obtain a catalyst solution. After aging for 1 hour, the catalyst solution was added to the pressure-resistant stainless steel reactor and heated to 80°C. Next, ethylene was charged into the pressure-resistant stainless steel reactor at a pressure of 1.0 MPa, and copolymerization was carried out at 80° C. while further adding 200 g of a toluene solution containing 50 g of 1,3-butadiene over a period of 90 minutes. Next, 1 mL of a 5% by mass solution of 2,2'-methylene-bis(4-ethyl-6-t-butylphenol) (NS-5) in isopropanol was added to the pressure-resistant stainless steel reactor to terminate the reaction. Next, separation was performed using a large amount of methanol and vacuum drying at 50° C. to obtain copolymer B.

[0183] Example 3: Preparation of Copolymer C 60 g of a toluene solution containing 15 g of 1,3-butadiene and 440 g of toluene were added to a thoroughly dried 2000 mL pressure-resistant stainless steel reactor. Ethylene was then added to the pressure-resistant stainless steel reactor at a pressure of about 1.0 MPa, and the system was replaced with ethylene three times. Meanwhile, in a glove box under a nitrogen atmosphere, 0.025 mmol of mono(bis(1,3-tert-butyldimethylsilyl)indenyl)bis(bis(dimethylsilyl)amide) gadolinium complex {1,3-[(t-Bu)Me2Si]2C9H5Gd[N(SiHMe2)2]2}, 0.025 mmol of trityl tetrakis(pentafluorophenyl)borate [Ph3CB(C6F5)4], and 0.75 mmol of triisobutylaluminum were charged into a glass vessel, and 10 mL of toluene was added to obtain a catalyst solution. After aging for 1 hour, the catalyst solution was added to the pressure-resistant stainless steel reactor and heated to 80°C. Next, ethylene was charged into the pressure-resistant stainless steel reactor at a pressure of 1.0 MPa, and copolymerization was carried out at 80° C. while further adding 300 g of a toluene solution containing 75 g of 1,3-butadiene over a period of 90 minutes. Next, 1 mL of a 5% by mass solution of 2,2'-methylene-bis(4-ethyl-6-t-butylphenol) (NS-5) in isopropanol was added to the pressure-resistant stainless steel reactor to terminate the reaction. Next, separation using a large amount of methanol and vacuum drying at 50° C. were carried out to obtain copolymer C.

[0184] Example 4: Preparation of Copolymer D A 2000 mL pressure-resistant stainless steel reactor that had been thoroughly dried was charged with 40 g of a toluene solution containing 10 g of 1,3-butadiene and 460 g of toluene. Ethylene was then added to the reactor at a pressure of about 1.0 MPa, and the system was replaced with ethylene three times. Meanwhile, in a glove box under a nitrogen atmosphere, 0.075 mmol of mono(bis(1,3-tert-butyldimethylsilyl)indenyl)bis(bis(dimethylsilyl)amide) gadolinium complex {1,3-[(t-Bu)Me2Si]2C9H5Gd[N(SiHMe2)2]2}, 0.025 mmol of trityl tetrakis(pentafluorophenyl)borate [Ph3CB(C6F5)4], and 0.25 mmol of triisobutylaluminum were charged into a glass vessel, and 10 mL of toluene was added to obtain a catalyst solution. After aging for 1 hour, the catalyst solution was added to the pressure-resistant stainless steel reactor and heated to 80°C. Next, ethylene was charged into the pressure-resistant stainless steel reactor at a pressure of 1.0 MPa, and copolymerization was carried out at 80° C. while further adding 200 g of a toluene solution containing 50 g of 1,3-butadiene over 180 minutes. Next, 1 mL of a 5% by mass solution of 2,2'-methylene-bis(4-ethyl-6-t-butylphenol) (NS-5) in isopropanol was added to the pressure-resistant stainless steel reactor to terminate the reaction. Then, separation using a large amount of methanol and vacuum drying at 50° C. were carried out to obtain copolymer D.

[0185] Comparative Example 1: Preparation of Copolymer E 60 g of a toluene solution containing 15 g of 1,3-butadiene and 340 g of toluene were added to a thoroughly dried 2000 mL pressure-resistant stainless steel reactor. Ethylene was then added to the pressure-resistant stainless steel reactor at a pressure of about 1.0 MPa, and the system was replaced with ethylene three times. Meanwhile, in a glove box under a nitrogen atmosphere, 0.040 mmol of mono(bis(1,3-tert-butyldimethylsilyl)indenyl)bis(bis(dimethylsilyl)amide) gadolinium complex {1,3-[(t-Bu)Me2Si]2C9H5Gd[N(SiHMe2)2]2}, 0.040 mmol of trityltetrakis(pentafluorophenyl)borate [Ph3CB(C6F5)4], and 1.0 mmol of triisobutylaluminum were charged into a glass vessel, and 25 mL of toluene was added to prepare a catalyst solution. After aging for 1 hour, the catalyst solution was added to the pressure-resistant stainless steel reactor and heated to 80°C. Next, ethylene was charged into the pressure-resistant stainless steel reactor at a pressure of 1.0 MPa, and copolymerization was carried out at 80° C. while further adding 300 g of a toluene solution containing 75 g of 1,3-butadiene over a period of 38 minutes. Next, 1 mL of a 5% by mass solution of 2,2'-methylene-bis(4-ethyl-6-t-butylphenol) (NS-5) in isopropanol was added to the pressure-resistant stainless steel reactor to terminate the reaction. Next, separation using a large amount of methanol and vacuum drying at 50° C. were performed to obtain copolymer E.

[0186] The resulting copolymer was subjected to the following measurements.

[0187] (1) Weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) Gel permeation chromatography [GPC: Tosoh HLC-8121GPC / HT, column: Tosoh GMH HR Using a 2-H(S)HT, detector: differential refractometer (RI), the weight average molecular weight (Mw), number average molecular weight (Mn) and molecular weight distribution (Mw / Mn) of the copolymer in terms of polystyrene were determined with monodisperse polystyrene as the standard. The measurement temperature was 40°C. The results are shown in Table 1.

[0188] (2) Ratio of 1,3-butadiene units and ethylene units The ratio (mol%) of 1,3-butadiene units and ethylene units in the copolymer is 1The results were calculated from the integral ratio of each peak in the H-NMR spectrum (100°C, d-tetrachloroethane standard: 6 ppm). The results are shown in Table 1.

[0189] (3) Confirmation of main chain structure The obtained copolymer was 13 The C-NMR spectrum was measured. 13 No peaks were observed in the range of 10 to 24 ppm in the C-NMR spectrum chart, confirming that the main chain of the synthesized copolymer was composed solely of acyclic structures.

[0190] (4) Endothermic peak energy Using a differential scanning calorimeter (DSC, manufactured by TA Instruments Japan, "DSCQ2000"), the obtained copolymer was heated from -150°C to 150°C at a rate of 10°C / min in accordance with JIS K 7121-1987. Then, the endothermic peak energy (ΔH1 (J / g)) in the range of 0°C to less than 100°C and the endothermic peak energy (ΔH2 (J / g)) in the range of 100°C to 150°C at that time (1st run) were measured. The results are shown in Table 1. For reference, DSC charts of the copolymers of Examples 1 to 4 and Comparative Example 1 are shown in Figures 1 to 5, respectively.

[0191] (5) Crystallinity In addition to the measurement of the endothermic peak energy, the crystalline melting energy (ΔH0) of 100% crystalline polyethylene was measured using a differential scanning calorimeter (DSC, manufactured by TA Instruments Japan, "DSCQ2000"). The degree of crystallinity (C1(%)) in the range of 0°C to less than 100°C was calculated from the ratio (ΔH1 / ΔH0) of the endothermic peak energy (ΔH1) of the copolymer in the range of 0°C to less than 100°C to the crystalline melting energy (ΔH0) of the polyethylene. The degree of crystallinity (C2(%)) in the range of 100°C to 150°C was calculated from the ratio (ΔH2 / ΔH0) of the endothermic peak energy (ΔH2) of the copolymer in the range of 100°C to 150°C to the crystalline melting energy (ΔH0) of the polyethylene. The results are shown in Table 1.

[0192] (6) Melting point The melting points of the copolymers were measured using a differential scanning calorimeter (DSC, manufactured by TA Instruments Japan, "DSCQ2000") in accordance with JIS K 7121-1987. The results are shown in Table 1.

[0193] (7) Glass transition temperature The glass transition temperature (Tg) of the copolymer was measured using a differential scanning calorimeter (DSC, manufactured by TA Instruments Japan, "DSCQ2000") in accordance with JIS K 7121-1987. The results are shown in Table 1.

[0194] [Table 1]

[0195] From Table 1, it can be seen that in the examples, copolymers were obtained in which the proportion of non-conjugated olefin units was 50 mol or more, and the crystallinity (C2) in the range of 100°C to 150°C, measured by differential scanning calorimetry (DSC), was greater than the crystallinity (C1) in the range of 0°C to less than 100°C. It is believed that the copolymers of the examples have high cut resistance and ozone resistance. [Industrial Applicability]

[0196] According to the present invention, a copolymer having excellent cut resistance and ozone resistance can be provided. Moreover, according to the present invention, it is possible to provide a rubber composition and a resin composition that are excellent in cut resistance and ozone resistance.

Claims

1. A copolymer consisting of only conjugated diene units and non-conjugated olefin units as monomer units, The proportion of the non-conjugated olefin units is 50 mol % or more, The crystallinity (C) measured by a differential scanning calorimeter (DSC) in the range of 100° C. to 150° C. 2 ) is the crystallinity (C 1 ) is larger than A copolymer, characterized in that the main chain is composed only of acyclic structures.

2. The crystallinity (C 2 2. The copolymer according to claim 1, wherein the ratio of 1:1 to 1:1 is 13% or more.

3. The crystallinity (C 1 3. The copolymer according to claim 1 or 2, wherein the ratio of the tungsten content to the total tungsten content is less than 13%.

4. The copolymer according to any one of claims 1 to 3, wherein the proportion of said conjugated diene units is 5 mol% or more and less than 50 mol%, and the proportion of said non-conjugated olefin units is 50 mol% or more and 95 mol% or less.

5. The copolymer according to any one of claims 1 to 4, which has a melting point of 100°C or higher as measured by a differential scanning calorimeter (DSC).

6. The copolymer according to any one of claims 1 to 5, having a weight average molecular weight in terms of polystyrene of 50,000 to 2,000,000.

7. The copolymer according to any one of claims 1 to 6, which has an endothermic peak energy of 35 J / g or more as measured by a differential scanning calorimeter (DSC).

8. The copolymer according to any one of claims 1 to 7, wherein the non-conjugated olefin units are acyclic non-conjugated olefin units.

9. The copolymer according to any one of claims 1 to 8, wherein the non-conjugated olefin units consist solely of ethylene units.

10. The copolymer according to any one of claims 1 to 9, wherein the conjugated diene units include 1,3-butadiene units and / or isoprene units.

11. The copolymer according to any one of claims 1 to 10, having a molecular weight distribution [Mw / Mn (weight average molecular weight / number average molecular weight)] of 1.00 to 4.

00.

12. A rubber composition comprising the copolymer according to any one of claims 1 to 11.

13. The rubber composition according to claim 12, further comprising a compound having two or more phenyl groups each having a branched alkyl group as an antioxidant.

14. A resin composition comprising the copolymer according to any one of claims 1 to 11.

15. The resin composition according to claim 14, further comprising a compound having two or more phenyl groups each having a branched alkyl group as an antioxidant.

Citation Information

Patent Citations

  • 1, 3 - butadiene copolymer of ethylene

    JP1989501633A

  • Unsaturated copolymer, preparation thereof and composition containing said copolymer

    JP1999080269A

  • Adhesive composition for flexible base board and flexible printed wiring board using the same

    JP2007161811A

  • Copolymer and method for producing the same, and rubber composition, crosslinked rubber composition, and tire

    JP2012131965A

  • Rubber composition for conveyor belt, and conveyor belt using the same

    JP2013079341A