Polarizing film, polarizing plate, optical laminate, elliptical polarizing plate, organic EL display device, and flexible image display device
The polarizing film with a photo-alignment film and a cured liquid crystal polarizer addresses adhesion issues by using polymers with photoreactive and polymerizable groups, enhancing optical properties and alignment stability.
Patent Information
- Application Number
- JP2020103151
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-15
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2040-06-15
AI Technical Summary
The adhesion between the alignment film and the polarizer in polarizing films is often inadequate, affecting the optical properties of the film.
A polarizing film comprising a photo-alignment film formed from a polymer containing structural units with photoreactive and polymerizable groups, and a polarizer made from a cured liquid crystal composition, where the polymerizable groups facilitate bonding between the alignment film and the polarizer.
The improved adhesion between the photo-alignment film and the polarizer results in enhanced optical properties, with the polarizer exhibiting high alignment order and stability, as evidenced by Bragg peaks in X-ray diffraction measurements.
Smart Images

Figure 0007576408000001 
Figure 0007576408000002 
Figure 0007576408000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing film, a polarizing plate including the same, an optical laminate, an elliptical polarizing plate, an organic EL display device, and a flexible image display device. [Background technology]
[0002] Polarizing plates are used in various image display panels such as liquid crystal display panels and organic electroluminescence (organic EL) display panels. As such polarizing plates, polarizing plates having a polarizer in which a dichroic dye such as iodine is aligned and adsorbed on a polyvinyl alcohol-based resin film, as well as polarizing films having a polarizer obtained by polymerizing a polymerizable liquid crystal compound applied to a substrate via a photoalignment film, are known. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2013-33249 A Summary of the Invention [Problem to be solved by the invention]
[0004] A polarizing film formed from a coating layer of a liquid crystal compound is often used in the form of a laminate having a polarizer and an alignment film used to form the polarizer. In a polarizing film having such a configuration, a decrease in adhesion between the alignment film and the polarizer can be a factor affecting the optical properties, etc., of the polarizing film. Therefore, an object of the present invention is to provide a polarizing film having excellent adhesion between a polarizer and an alignment film. [Means for solving the problem]
[0005] The present inventors have conducted extensive research to solve the above problems and have completed the present invention. That is, the present invention provides the following preferred embodiments. [1] A polarizing film including a photo-alignment film and a polarizer adjacent to the photo-alignment film, the photoalignment film is formed from a polymer including a structural unit having a photoreactive group and a structural unit having a polymerizable group, The polarizer is a cured product of a liquid crystal composition containing a liquid crystal compound and a dichroic dye, and the polarizing film contains a structural unit having a polymerizable group derived from the liquid crystal compound or the dichroic dye. [2] The polarizing film according to [1], wherein the photoreactive group is a group that undergoes a dimerization reaction or an isomerization reaction. [3] The polarizing film according to [1] or [2], wherein the polymer forming the photoalignment film further contains a structural unit having a carboxy group. [4] The polarizing film according to any one of [1] to [3], wherein the polymer forming the photoalignment film has a weight average molecular weight of 20,000 or more and 150,000 or less. [5] The polymer forming the photoalignment film is represented by the formula (II): [ka] [In formula (II), Ma, Mb and Mc represent monomer units forming the backbone of the copolymer; m, n and l represent the mole fractions of the copolymer and are equal to or less than 0 in each case. <m<1かつ0<n<1かつ0<l<1であり; SPCRa, SPCRb, and SPCRc each independently represent a spacer unit; Ring A, ring B and ring C are each independently an unsubstituted or substituted alicyclic hydrocarbon or an unsubstituted or substituted aromatic ring; X is a single covalent bond, an alkylene chain having 1 to 10 carbon atoms, or a cycloalkylene chain having 3 to 8 carbon atoms; Y is -O-CO-CH=CH2- (either bond may be bonded to ring B), or -N=N-; Z is selected from the group consisting of a single covalent bond; an alkylene chain having 1 to 10 carbon atoms, which is unsubstituted or substituted with a hydroxyl group and / or a carbonyl group; a cycloalkylene chain having 3 to 8 carbon atoms; -O-; -COO-; and combinations thereof; R1 is a phenyl group having at least one substituent selected from an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group, and a halogen atom; R 2 is -CW=CH2, or -V-CW=CH2 (wherein W is a hydrogen atom or a methyl group, and V is -O-CO- or -CO-). The polarizing film according to any one of [1] to [4], which has a repeating unit represented by the following formula: [6] The polarizing film according to any one of [1] to [5], wherein the dichroic dye comprises an azo dye. [7] The polarizing film according to any one of [1] to [6], wherein the polarizer contains a polymer of a polymerizable liquid crystal compound. [8] The polarizing film according to any one of [1] to [7], wherein the polarizer exhibits a Bragg peak in X-ray diffraction measurement. [9] A polarizing plate comprising the polarizing film according to any one of [1] to [8] and a substrate disposed on the photo-alignment film side of the polarizing film.
[10] An optical laminate comprising the polarizing plate according to [9] and a layer attached to the polarizer side of the polarizing plate via a pressure-sensitive adhesive layer.
[11] An elliptical polarizing plate comprising the polarizing film according to any one of [1] to [8] and a retardation layer having a quarter-wave plate function.
[12] An organic electroluminescence display device comprising the elliptically polarizing plate according to
[11] .
[13] A flexible image display device comprising the elliptically polarizing plate according to
[11] .
[14] The flexible image display device according to
[13] , further comprising a window and a touch sensor. Effect of the Invention
[0006] According to the present invention, it is possible to provide a polarizing film having excellent adhesion between a polarizer and an alignment film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] Hereinafter, the embodiments of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiments described here, and various modifications can be made without departing from the spirit of the present invention.
[0008] [Polarizing film] The polarizing film of the present invention includes a photo-alignment film and a polarizer adjacent to the photo-alignment film, and is essentially composed of the photo-alignment film and the polarizer. In this specification, a laminate consisting of the photo-alignment film and the polarizer laminated adjacent to the photo-alignment film is referred to as a polarizing film, and when a substrate is disposed on the photo-alignment film side in addition to the photo-alignment film and the polarizer adjacent to the photo-alignment film, a laminate consisting of each layer from the substrate to the polarizer is referred to as a polarizing plate.
[0009] The photo-alignment film constituting the polarizing film of the present invention is formed from a polymer containing a structural unit having a photoreactive group and a structural unit having a polymerizable group, and is preferably formed from a copolymer containing a structural unit having a photoreactive group and a structural unit having a polymerizable group. In the present invention, the polymer and the copolymer are usually (co)polymers. In the polymer forming the photo-alignment film, the structural unit having a photoreactive group contributes to imparting liquid crystal alignment ability by the action of light, and the structural unit having a polymerizable group contributes to improving adhesion with a polarizer formed on the photo-alignment film.
[0010] In one embodiment of the present invention, the structural unit having a photoreactive group (hereinafter also referred to as "structural unit (i)") is derived from a monomer having at least one photoreactive group. The photoreactive group refers to a group that generates liquid crystal alignment ability upon light irradiation. Specifically, it refers to a group that generates a photoreaction that is the origin of liquid crystal alignment ability upon light irradiation, such as a dimerization reaction, an isomerization reaction, or a photodecomposition reaction, and induces alignment of polymer molecules. The photoreactive group possessed by the structural unit (i) may be one type or two or more types.
[0011] The dimerization reaction is a reaction in which an addition reaction occurs between two groups by the action of light, typically forming a ring structure. The group that causes such a dimerization reaction is a group containing a carbon-carbon double bond (C=C bond) or a carbon-oxygen double bond (C=O bond) that causes a dimerization reaction by light irradiation, and examples thereof include a group having a cinnamoyl structure, a group having a chalcone structure, a group having a coumarin structure, a group having a benzophenone structure, and a group having an anthracene structure. Among them, from the viewpoint of relatively small amount of polarized light irradiation required for photo-alignment and easy production of a photo-alignment film having excellent thermal stability and stability over time, a group having a cinnamoyl structure and a group having a chalcone structure are preferred, and a group having a cinnamoyl structure is more preferred.
[0012] An isomerization reaction is a reaction in which a single compound is transformed into another isomer, such as stereoisomerization or structural isomerization, by the action of light. Groups that cause such an isomerization reaction include groups containing a nitrogen-nitrogen double bond (N=N bond) or a carbon-carbon double bond (C=C bond) that induces an isomerization reaction upon irradiation with light, such as a group having an azobenzene structure, a group having a stilbene structure, a group having a hydrazono-β-ketoester structure (skeleton), and a group having a spiropyran structure (skeleton).
[0013] The photodecomposition reaction is a reaction in which polymer chains are cut by the action of light, resulting in the development of anisotropy.
[0014] In the present invention, the photoreactive group is preferably a group that causes a dimerization reaction and a group that causes an isomerization reaction, and more preferably a group that causes a dimerization reaction. The group that causes a dimerization reaction and the group that causes an isomerization reaction are preferred from the viewpoint of reactivity and cost. In particular, with regard to reactivity, it is important to react photoreactively without reacting structural units having polymerizable groups described later.
[0015] In one embodiment of the present invention, the structural unit having a polymerizable group (hereinafter also referred to as "structural unit (ii)") is derived from a monomer having at least one polymerizable group. The polymerizable group means a group involved in a polymerization reaction, and includes a thermally polymerizable group and a photopolymerizable group, and the polymerizable group contained in the structural unit having a polymerizable group is preferably a photopolymerizable group. The structural unit (ii) may have one type of polymerizable group or two or more types of polymerizable groups.
[0016] Examples of the polymerizable group constituting the structural unit (ii) include a vinyl group, a vinyloxy group, a 1-chlorovinyl group, an isopropenyl group, a 4-vinylphenyl group, a (meth)acryloyl group, a (meth)acryloyloxy group, an oxiranyl group, and an oxetanyl group. Among them, from the viewpoint of ease of reaction control and improvement of adhesion with a polarizer, a (meth)acryloyl group, a (meth)acryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group are preferable, a (meth)acryloyl group and a (meth)acryloyloxy group are more preferable, and a (meth)acryloyloxy group is even more preferable. In this specification, "(meth)acryloyl" refers to methacryloyl and acryloyl.
[0017] When the photo-alignment film is formed from a polymer containing a structural unit (ii) having a polymerizable group, a polarizing film having excellent adhesion between the photo-alignment film and a polarizer laminated adjacent thereto can be formed. One of the reasons for this effect is that when a polarizer, which is a cured product of a liquid crystal composition, is formed, the polymerizable group contained in the photo-alignment film reacts with the polymerizable group of the liquid crystal compound or liquid crystal substance such as a dichroic dye for forming the polarizer and bonds with the polymerizable group of the liquid crystal compound or liquid crystal substance such as a dichroic dye for forming the polarizer. Therefore, when the dichroic dye or polymerizable liquid crystal compound forming the polarizer has the same polymerizable group as the polymerizable group of the polymer, the adhesion between the polarizer and the photo-alignment film is more likely to be improved.
[0018] In the present invention, the polymer forming the photo-alignment film has an unreacted polymerizable group as the structural unit (ii). The structural unit (ii) is derived from a monomer having the polymerizable group. In the polymer, the polymerizable group of at least a part of the monomers forming the polymer remains unreacted. In the structural unit derived from the monomer having the polymerizable group, all of the polymerizable groups may remain unreacted. When a sufficient proportion of unreacted polymerizable groups are present in the polymer, when a polarizer is formed after the formation of the photo-polarizing film, a sufficient amount of polymerizable groups that can react simultaneously with the polymerization reaction of the liquid crystal substance for forming the polarizer can be present in the photo-alignment film, and therefore the adhesion between the photo-alignment film and the polarizer is likely to be improved.
[0019] Since it is easy to form an alignment film that exhibits high liquid crystal alignment ability while having excellent adhesion to a polarizer, the polymer that forms the photoalignment film in the present invention is preferably a polymer having structural units (i) and (ii), and more preferably a polymer in which a photoreactive group and a polymerizable group are located at the ends of the polymer side chains, respectively.
[0020] Examples of the polymer containing the structural unit (i) and the structural unit (ii) include a polymer obtained by copolymerizing a monomer that derives the structural unit (i) with a monomer that derives the structural unit (ii), or by introducing a polymerizable group that the structural unit (ii) has into a (co)polymer that contains the structural unit (i). Examples of such a polymer include a copolymer having a structure represented by the following formula (I) as a repeating unit.
[0021] [ka] [In formula (I), Mb and Mc represent monomer units forming the backbone of the copolymer; n and l represent the mole fractions of the copolymer and are equal to 0 in each case. <n<1かつ0<l<1であり; SPCRb and SPCRc each independently represent a spacer unit; Ring B and Ring C are each independently an unsubstituted or substituted alicyclic hydrocarbon or an unsubstituted or substituted aromatic ring; Y is -O-CO-CH=CH2- (either bond may be bonded to ring B), or -N=N-; Z is selected from the group consisting of a single covalent bond; an alkylene chain having 1 to 10 carbon atoms, which is unsubstituted or substituted with a hydroxyl group and / or a carbonyl group; a cycloalkylene chain having 3 to 8 carbon atoms; -O-; -COO-; and combinations thereof; R 1 is a phenyl group having at least one substituent selected from an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group, and a halogen atom; R 2 is -CW=CH2, or -V-CW=CH2 (wherein W is a hydrogen atom or a methyl group, and V is -O-CO- or -CO-).
[0022] In formula (I), the structures of Mb and Mc, which are monomer units forming the main chain of the copolymer, include, for example, those selected from the group consisting of (meth)acrylic acid ester units represented by formula (M-1) or formula (M-2); (meth)acrylamide units represented by formula (M-3) or formula (M-4); vinyl ether units represented by formula (M-5) or formula (M-6); (methyl)styrene units represented by formula (M-7) or formula (M-8), and vinyl ester units represented by formula (M-9) or formula (M-10). In formulas (M-1) to (M-10), * represents a bond to the spacer units SPCRb and SPCRc. The main chain of the copolymer in formula (I) is preferably composed of units selected from the above group, and more preferably composed of units selected from the group consisting of (meth)acrylic acid ester units and (meth)acrylamide units. The term "copolymer main chain" used herein refers to the longest molecular chain among the molecular chains contained in the copolymer. [ka]
[0023] In formula (I), examples of the spacer units SPCRb and SPCRc include a carbonyloxy group (ester bond), an oxygen atom (ether bond), an imide group (imide bond), a carbonylimino group (amide bond), an iminocarbonylimino group (urethane bond), a divalent aliphatic hydrocarbon group which may have a substituent, a divalent aromatic hydrocarbon group which may have a substituent, and a divalent group formed by combining these. Specific examples of the divalent aromatic hydrocarbon group which may have a substituent include a phenylene group, a 2-methoxy-1,4-phenylene group, a 3-methoxy-1,4-phenylene group, a 2-ethoxy-1,4-phenylene group, a 3-ethoxy-1,4-phenylene group, and a 2,3,5-trimethoxy-1,4-phenylene group. Among these, the linking group is preferably an aliphatic hydrocarbon group, and more preferably an alkanediyl group having 1 to 11 carbon atoms which may have a substituent. Examples of the alkanediyl group include methylene, ethylene, trimethylene, tetramethylene, pentamethylene, hexamethylene, heptamethylene, octamethylene, nonamethylene, decamethylene, and undecamethylene groups, which may be linear or branched. The alkanediyl group may have a substituent. The substituent is, for example, an alkoxy group having 1 to 4 carbon atoms.
[0024] In formula (I), examples of ring B and ring C include ring structures represented by formulae (X-1) to (X-5). [ka]
[0025] In the above structure, X 1 ~X 38 are each independently a hydrogen atom, an alkyl group, an alkoxy group, a halogen atom, or a cyano group. 1 ~X 38 The alkyl group represented by X is an alkyl group having 1 to 4 carbon atoms. 1 ~X 38The alkoxy group represented by X includes an alkoxy group having 1 to 4 carbon atoms. 1 ~X 38 are each preferably a hydrogen atom or a halogen atom, more preferably a hydrogen atom.
[0026] Ring B and ring C are preferably a ring structure represented by formula (X-1) or (X-5), more preferably a ring structure represented by formula (X-1).
[0027] In formula (I), R 1 is preferably an alkyl group having 1 to 6 carbon atoms, or a phenyl group having at least one substituent selected from a cyano group and a halogen atom, more preferably an alkyl group having 1 to 6 carbon atoms, or a phenyl group substituted with a cyano group, and even more preferably an alkyl group having 1 to 6 carbon atoms. 1 The alkyl group is preferably an alkyl group having 1 to 4 carbon atoms, and more preferably a methyl group.
[0028] In formula (I), R 2 is preferably -CW=CH2, or -V-CW=CH2 (wherein W is a hydrogen atom or a methyl group, and V is -O-CO- or -CO-).
[0029] In formula (I), n and l are the molar fractions of the structural unit (i) and the structural unit (ii) relative to all structural units of the polymer forming the photo-alignment film, and preferably satisfy the relationships of 0.1≦n≦0.9 and 0.1≦l≦0.9. It is preferable from the viewpoints of alignment and adhesion that the molar fractions of the structural unit (i) and the structural unit (ii) are within the above ranges.
[0030] Formula (I) is a schematic representation of the monomer that derives the structural unit (i) and the monomer that derives the structural unit (ii) being contained in a molar ratio of n:l, and does not necessarily represent that the monomer that derives the structural unit (i) and the monomer that derives the structural unit (ii) are alternately bonded to form a copolymer. That is, formula (I) may include any copolymer in which the monomer that derives the structural unit (i) and the monomer that derives the structural unit (ii) are polymerized in a molar ratio of n:l, such as an alternating type, a block type, a random type, or a graft type.
[0031] In one embodiment of the present invention, the polymer forming the photoalignment film preferably further contains a structural unit having a carboxy group (hereinafter also referred to as "structural unit (iii)") in addition to the structural unit (i) and the structural unit (ii).
[0032] When the photo-alignment film contains the structural unit (iii), the polymer forming the photo-alignment film is preferably a polymer having the structural unit (i), the structural unit (ii) and the structural unit (iii), and more preferably a polymer having a photoreactive group, a polymerizable group and a carboxyl group at the end of the polymer side chain, respectively. When the polymer has such a structure, an alignment film having excellent adhesion to a polarizer is easily formed.
[0033] Examples of the polymer containing the structural unit (i), the structural unit (ii) and the structural unit (iii) include a polymer obtained by copolymerizing a monomer which derives the structural unit (i), a monomer which derives the structural unit (ii) and a monomer which derives the structural unit (iii), or by introducing a polymerizable group possessed by the structural unit (ii) into a (co)polymer containing the structural unit (i) and / or the structural unit (iii). Examples of such a polymer include a copolymer having a structure represented by the following formula (II) as a repeating unit.
[0034] [ka] [In formula (II), Ma, Mb and Mc represent monomer units forming the backbone of the copolymer; m, n and l represent the mole fractions of the copolymer and are equal to or less than 0 in each case. <m<1かつ0<n<1かつ0<l<1であり; SPCRa, SPCRb, and SPCRc each independently represent a spacer unit; Ring A, ring B and ring C are each independently an unsubstituted or substituted alicyclic hydrocarbon or an unsubstituted or substituted aromatic ring; X is a single covalent bond, an alkylene chain having 1 to 10 carbon atoms, or a cycloalkylene chain having 3 to 8 carbon atoms; Y is -O-CO-CH=CH2- (either bond may be bonded to ring B), or -N=N-; Z is selected from the group consisting of a single covalent bond; an alkylene chain having 1 to 10 carbon atoms, which is unsubstituted or substituted with a hydroxyl group and / or a carbonyl group; a cycloalkylene chain having 3 to 8 carbon atoms; -O-; -COO-; and combinations thereof; R 1 is a phenyl group having at least one substituent selected from an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group, and a halogen atom; R 2 is -CW=CH2, or -V-CW=CH2 (wherein W is a hydrogen atom or a methyl group, and V is -O-CO- or -CO-).
[0035] In formula (II), the structures of Ma, Mb and Mc which are monomer units forming the main chain of the copolymer include the same structures as those exemplified as the structures of Mb and Mc in formula (I).
[0036] In formula (II), the spacer units SPCRa, SPCRb and SPCRc include the same structures as those exemplified as the structures of SPCRb and SPCRc in formula (I).
[0037] In formula (II), ring A, ring B and ring C include the same structures as those exemplified as the structures of ring B and ring C in formula (I). In formula (II), ring A is preferably a ring structure represented by formula (X-1), and ring B and ring C are preferably ring structures represented by formula (X-1) or (X-5), more preferably ring structures represented by formula (X-1).
[0038] R in formula (II) 1 and R 2 As the group, R in formula (II) 1 and R 2 As the structure of the compound, the same structures as those exemplified above can be mentioned.
[0039] In formula (II), m, n, and l are the molar fractions (m+n+l=1) of the structural unit (iii), the structural unit (i), and the structural unit (ii) relative to the total structural units of the polymer forming the photo-alignment film, and preferably satisfy the relationships of 0.1≦m≦0.8, 0.1≦n≦0.5, and 0.1≦l≦0.5, and more preferably satisfy the relationships of 0.3≦m≦0.8, 0.1≦n≦0.3, and 0.1≦l≦0.3. It is preferable from the viewpoint of alignment and adhesion that the molar fractions of the structural unit (i), the structural unit (ii), and the structural unit (iii) are within the above ranges.
[0040] Formula (II) is a schematic representation of the molar ratio of the monomer that derives the structural unit (i), the monomer that derives the structural unit (ii), and the monomer that derives the structural unit (iii) being n:l:m, and does not necessarily represent that the monomer that derives the structural unit (i), the monomer that derives the structural unit (ii), and the monomer that derives the structural unit (iii) are alternately bonded to form a copolymer. That is, formula (I) may include any copolymer obtained by polymerizing the monomer that derives the structural unit (i), the monomer that derives the structural unit (ii), and the monomer that derives the structural unit (iii) in a molar ratio of n:l:m, such as an alternating type, block type, random type, or graft type.
[0041] In one embodiment of the present invention, the polymer that forms the photoalignment film may contain structural units other than the structural units (i), (ii), and (iii) (hereinafter also referred to as "other structural units"), so long as the effects of the present invention are not adversely affected.
[0042] The polymer forming the photo-alignment film preferably has a weight-average molecular weight of 20,000 or more and 150,000 or less. When the weight-average molecular weight is equal to or more than the above lower limit, the solvent resistance is improved, and a photo-alignment film exhibiting high liquid crystal alignment ability is easily obtained while ensuring high adhesion with a polarizer formed later on the photo-alignment film. In addition, after the photo-alignment film is produced, alignment tends to be more likely to occur when a liquid crystal composition (composition for forming a polarizer) is applied. Furthermore, the present inventors have found that, within the above range, the larger the weight-average molecular weight of the polymer forming the photo-alignment film, the higher the liquid crystal alignment ability tends to be, and even if the processing temperature when forming the photo-alignment film is relatively high, excellent liquid crystal alignment ability can be exhibited. In the present invention, the weight-average molecular weight of the polymer forming the photo-alignment film is more preferably 30,000 or more, more preferably 50,000 or more, and more preferably 140,000 or less, and more preferably 130,000 or less. The weight average molecular weight of the polymer can be measured and calculated using a measuring device such as gel permeation chromatography.
[0043] The polymer (hereinafter also referred to as "polymer (I')") forming the photo-alignment film containing the structural units (i) and (ii) can be produced by mixing a predetermined amount of a monomer that derives the structural unit (i) and a monomer that derives the structural unit (ii), and if necessary, a monomer that derives the structural unit (iii) and a monomer that derives other structural units in a solventless or solvent and copolymerizing them, or by introducing a polymerizable group possessed by the structural unit (ii) during (co)polymerization of the monomer that derives the structural unit (i) and / or the monomer that derives the structural unit (iii). As the copolymerization method, a method conventionally known in the art may be adopted, and examples thereof include chain polymerization such as radical polymerization, anionic polymerization, and cationic polymerization, and coordination polymerization. The polymerization conditions are appropriately determined so as to obtain a polymer having a desired molecular weight depending on the type and amount of the monomer used.
[0044] When polymerization is performed in a solvent, known organic solvents can be used without any particular limitation. Specific examples of the solvent include alcohol-based solvents such as ethanol, propanol, butanol, ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, cyclopentanone, ester-based solvents such as ethyl acetate, butyl acetate, propylene glycol monomethyl ether acetate, ether-based solvents such as diethyl ether, diglyme, hydrocarbon-based solvents such as hexane, cyclohexane, methylcyclohexane, toluene, xylene, nitrile-based solvents such as acetonitrile, and amide-based solvents such as N-methyl-2-pyrrolidone and dimethylacetamide. Any of these solvents may be used alone, or two or more may be used in combination.
[0045] A polymerization initiator may be used in the polymerization. The polymerization initiator may be appropriately selected from known polymerization initiators, and examples thereof include azo-based polymerization initiators such as azobisisobutyronitrile (AIBN), diethyl-2,2'-azobisisobutyrate (V-601), 2,2'-azobis(2,4-dimethylvaleronitrile), and dimethylazobismethylpropionate, peroxide-based polymerization initiators such as benzoyl peroxide, hydrogen peroxide, and lauroyl peroxide, and persulfate-based polymerization initiators such as potassium persulfate and ammonium persulfate. Any of these polymerization initiators may be used alone, or two or more of them may be used in combination.
[0046] The polymerization conditions are appropriately determined depending on the type and amount of the monomer used, so as to obtain a polymer having a desired molecular weight. For example, the temperature during polymerization may be appropriately set depending on the type of monomer, polymerization solvent, polymerization initiator, etc. used, but is preferably in the range of 40 to 150°C, more preferably 50 to 120°C.
[0047] The photo-alignment film is obtained by applying a composition containing a polymer (I') and a solvent capable of dissolving the polymer (I') (hereinafter also referred to as "photo-alignment film-forming composition") to a surface of a substrate or the like on which the photo-alignment film is to be formed, drying to remove the solvent, and then irradiating with polarized light (preferably polarized UV). The photo-alignment film-forming composition may contain a polymer material such as polyvinyl alcohol or polyimide, or a photosensitizer, as long as the properties of the photo-alignment film are not significantly impaired.
[0048] The content of the polymer (I') in the composition for forming a photo-alignment film can be appropriately adjusted depending on the structure of the polymer (I') and the thickness of the desired photo-alignment film, but is preferably at least 0.1 mass% in terms of solid content relative to the mass of the composition for forming a photo-alignment film, and more preferably in the range of 0.3 to 10 mass%. In this specification, the solid content refers to the total amount of components obtained by excluding volatile components such as solvents from the composition for forming a photo-alignment film. Hereinafter, in the composition for forming a polarizer, etc., it also refers to the total amount of components obtained by excluding volatile components such as solvents from the target composition.
[0049] The solvent used in the photo-alignment film-forming composition can be appropriately selected according to the type of polymer (I') used. For example, water; alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, and propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, and ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl amyl ketone, and methyl isobutyl ketone; aliphatic hydrocarbon solvents such as pentane, hexane, and heptane; aromatic hydrocarbon solvents such as toluene and xylene, and nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran and dimethoxyethane; chlorine-substituted hydrocarbon solvents such as chloroform and chlorobenzene; and the like. These solvents may be used alone or in combination of two or more.
[0050] Examples of a method for applying the composition for forming a photoalignment film to a substrate or the like include known methods such as application methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography.
[0051] The method for drying and removing the solvent includes natural drying, ventilation drying, heat drying, reduced pressure drying, etc. By this, a dry coating film is formed.
[0052] The method of irradiating polarized light may be a method of directly irradiating a dried coating film obtained by removing the solvent from the composition for forming a photo-alignment film with polarized light, or a method of irradiating polarized light from the side of a substrate or the like on which a dried coating film is formed, and then irradiating the polarized light through the substrate. In addition, it is particularly preferable that the polarized light is substantially parallel light. The wavelength of the irradiated polarized light is preferably in a wavelength range in which the photoreactive group of the polymer (I') can absorb light energy. Specifically, UV (ultraviolet light) having a wavelength in the range of 250 to 400 nm is particularly preferable.
[0053] Examples of light sources used for the polarized light irradiation include xenon lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, and ultraviolet lasers such as KrF and ArF, and high-pressure mercury lamps, ultra-high-pressure mercury lamps, and metal halide lamps are more preferred. These lamps are preferred because they have a high emission intensity of ultraviolet light with a wavelength of 313 nm. Polarized light can be irradiated by irradiating the light from the light source through an appropriate polarizer. As such a polarizer, a polarizing filter, a polarizing prism such as Glan-Thompson or Glan-Taylor, or a wire grid type polarizer can be used.
[0054] If masking is performed during the irradiation of polarized light, a plurality of regions (patterns) in which the liquid crystal alignment directions are different can be formed.
[0055] The thickness of the photo-alignment film is preferably 10 to 5000 nm, more preferably 10 to 1000 nm, and further preferably 30 to 300 nm. When the thickness of the photo-alignment film is in the above range, the film can exert an alignment control force while exhibiting good adhesion to the polarizer, and a polarizer can be formed with high alignment order.
[0056] The polarizer constituting the polarizing film of the present invention is a cured product of a liquid crystal composition, i.e., a coating layer formed from a liquid crystal composition. The liquid crystal composition forming the polarizer (hereinafter, also referred to as a "polarizer-forming composition") contains a liquid crystal compound and a dichroic dye.
[0057] The dichroic dye means a dye having different absorbance in the long axis direction of the molecule and absorbance in the short axis direction. The dichroic dye usable in the present invention is not particularly limited as long as it has the above-mentioned properties, and may be a dye or a pigment. In addition, two or more kinds of dyes or pigments may be used in combination, or a dye and a pigment may be used in combination. In addition, the dichroic dye may have polymerizability or liquid crystal properties.
[0058] In one embodiment of the present invention, the dichroic dye has a maximum absorption wavelength (λ ) in the range of 300 to 700 nm. MAX ) is preferable. Examples of such dichroic dyes include acridine dyes, oxazine dyes, cyanine dyes, naphthalene dyes, azo dyes, and anthraquinone dyes. Among them, azo dyes are suitable for producing a polarizer with excellent polarization performance because of their high linearity. Therefore, in one embodiment of the present invention, the dichroic dye contained in the polarizer-forming composition that forms the polarizer is preferably an azo dye.
[0059] Examples of the azo dye include monoazo dyes, bisazo dyes, trisazo dyes, tetrakisazo dyes, and stilbene azo dyes. Of these, bisazo dyes and trisazo dyes are preferred, and examples thereof include compounds represented by formula (1). K 1 (-N=NK 2 ) p -N=NK 3 (1) [In formula (1), K 1 and K. 3 each independently represents a phenyl group which may have a substituent, a naphthyl group which may have a substituent, or a monovalent heterocyclic group which may have a substituent. 2 represents a p-phenylene group which may have a substituent, a naphthalene-1,4-diyl group which may have a substituent, or a divalent heterocyclic group which may have a substituent. p represents an integer of 1 to 4. When p is an integer of 2 or more, a plurality of K 2may be the same or different. The -N=N- bond may be replaced with a -C=C-, -COO-, -NHCO-, or -N=CH- bond as long as the compound exhibits absorption in the visible region.
[0060] In formula (1), examples of the monovalent heterocyclic group include groups in which one hydrogen atom has been removed from a heterocyclic compound such as quinoline, thiazole, benzothiazole, thienothiazole, imidazole, benzimidazole, oxazole, benzoxazole, etc. Examples of the divalent heterocyclic group include groups in which two hydrogen atoms have been removed from the above-mentioned heterocyclic compounds.
[0061] K in Equation (1) 1 and K. 3 Phenyl, naphthyl and monovalent heterocyclic groups in 2 Examples of the substituent that the p-phenylene group, naphthalene-1,4-diyl group, and divalent heterocyclic group may have include an alkyl group having 1 to 20 carbon atoms, an alkyl group having 1 to 20 carbon atoms and having a polymerizable group, an alkenyl group having 1 to 4 carbon atoms; an alkoxy group having 1 to 20 carbon atoms such as a methoxy group, an ethoxy group, and a butoxy group, an alkoxy group having 1 to 20 carbon atoms and having a polymerizable group; a fluorinated alkyl group having 1 to 4 carbon atoms such as a trifluoromethyl group; a cyano group; a nitro group; a halogen atom; and a substituted or unsubstituted amino group such as an amino group, a diethylamino group, or a pyrrolidino group (the substituted amino group means an amino group having one or two alkyl groups having 1 to 6 carbon atoms, an amino group having one or two alkyl groups having 1 to 6 carbon atoms and having a polymerizable group, or an amino group in which two substituted alkyl groups are bonded to each other to form an alkanediyl group having 2 to 8 carbon atoms. An unsubstituted amino group is -NH2). Examples of the polymerizable group include an acryloyl group, a methacryloyl group, an acryloyloxy group, and a methacryloyloxy group.
[0062] Examples of the azo dye represented by formula (1) include compounds represented by any of the following formulas (1-1) to (1-8). These azo dyes may be used alone or in combination of two or more. [ka] [In formulas (1-1) to (1-8), B 1 ~B 30 each independently represents a hydrogen atom, an alkyl group having 1 to 6 carbon atoms, an alkenyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, a nitro group, a substituted or unsubstituted amino group (the substituted amino group and the unsubstituted amino group are defined above), a chlorine atom, or a trifluoromethyl group. n1 to n4 each independently represent an integer of 0 to 3. If n1 is 2 or more, multiple B 2 may be the same or different, If n2 is 2 or more, multiple B 6 may be the same or different, If n3 is 2 or more, multiple B 9 may be the same or different, If n4 is 2 or more, multiple B 14 may be the same or different.]
[0063] The polarizer constituting the polarizing film of the present invention contains a structural unit having a polymerizable group derived from a liquid crystal compound or a dichroic dye, and when the polarizer contains the structural unit, a bond can be formed between the structural unit (ii) constituting the polymer (I') forming the photo-alignment film and the polymerizable group, making it easier to form a polarizing film having excellent adhesion between the photo-alignment film and the polarizer. Therefore, the dichroic dye in the present invention may be a dichroic dye having a polymerizable group.
[0064] When the dichroic dye has a polymerizable group, examples of the polymerizable group include groups exemplified as the polymerizable group of the structural unit (ii) constituting the polymer (I'). Among them, from the viewpoint of ease of reaction control, preferred are (meth)acryloyl group, (meth)acryloyloxy group, vinyloxy group, oxiranyl group and oxetanyl group, more preferred are (meth)acryloyl group and (meth)acryloyloxy group, and even more preferred are (meth)acryloyloxy group. The polymerizable group in the dichroic dye may be one type alone or a combination of two or more types, but is preferably the same polymerizable group as the polymerizable group of the structural unit (ii). The number of polymerizable groups in the dichroic dye is not particularly limited, and may be one or more.
[0065] The dichroic dye having a polymerizable group may be a compound represented by the above formula (1) having a polymerizable group, or a compound represented by the following formula (2): [ka] [In formula (2), m represents an integer of 0 to 3; A 1 , A 2 and A 3 each independently represents a divalent aromatic group which may have a substituent; L 1 and L 2 are each independently a single bond, -CH2-, -CH2CH2-, -O-, -CH2O-, -OCH2-, -CO-, -COO-, -OCO-, -OCOO-, -CR c =CR d -, -C≡C-, -CR c =N-, -CONR c -, -NR c CO- or -N=N-, where R c and R d each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; Z 1 represents a polymerizable group; Z 2 represents a hydrogen atom or a polymerizable group; Q 1and Q 2 each independently represents a linear or branched alkylene group having 1 to 20 carbon atoms which may have a substituent, an alkenylene group having 1 to 20 carbon atoms which may have a substituent, or an alkynylene group having 1 to 20 carbon atoms which may have a substituent, and -CH2- contained in these alkylene groups, alkenylene groups, or alkynylene groups is -O-, -S-, or NR e -, where R e represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms; T 1 is a single bond, -O-, -S-, -CO-, -COO-, -OCO-, -OCOO-, or -CONR f - or -NR f CO- stands for T 2 is a single bond, -O-, -S-, -CO-, -COO-, -OCO-, -OCOO-, -CONR f -, -NR f CO- or -NR g -, where R f and R g each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, R g The alkyl group represented by Q 1 or Q 2 A may form a ring with 1 -(L 1 -A 2 ) m -L 2 -A 3 At least one -A X1 -N=NA X2 -(In the formula, A X1 and A X2 Each of T represents a divalent aromatic group, 2 Ga-NR g -Z if 2 represents a hydrogen atom] and the like.
[0066] The content of the dichroic dye may be appropriately determined depending on the type of the dichroic dye used. From the viewpoint of easily increasing the adhesion to the photo-alignment film and the dichroic ratio, the content may be, for example, 1 to 99 parts by mass, preferably 2 parts by mass or more, more preferably 3 parts by mass or more, relative to 100 parts by mass of the solid content of the composition for forming a polarizing film. In addition, from the viewpoint of easily increasing the degree of orientation order of the polarizer, the content is preferably 80 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 25 parts by mass or less, and particularly preferably 10 parts by mass or less. When a plurality of dichroic dyes are included as the dichroic dye, it is preferable that the total amount of all the dichroic dyes included in the composition for forming a polarizer is within the above range. The dichroic ratio is the ratio of the absorption intensities of two linearly polarized lights that vibrate perpendicularly to each other when they enter a polarizer. It is defined as the ratio (AV / AH) of the absorbance (AV) along the extinction axis (measured at normal incidence) to the absorbance (AH) along the transmission axis. The transmission axis (polarization axis) refers to the polarization direction of the component that is transmitted through the polarizing film out of the light incident on the polarizing film, and the extinction axis (absorption axis) refers to the polarization direction of the component that is absorbed by the polarizing film out of the light incident on the polarizing film.
[0067] The structural unit having a polymerizable group in the polarizer may be derived from a liquid crystal compound having a polymerizable group. In one embodiment of the present invention, the composition for forming a polarizer preferably contains a polymerizable liquid crystal compound from the viewpoint of easily improving adhesion to a photo-alignment film and easily increasing alignment. Here, the liquid crystal compound refers to a liquid crystal substance exhibiting liquid crystallinity, and the dichroic dye having a polymerizable group described above can also be a type of liquid crystal substance having a polymerizable group, but the polymerizable liquid crystal compound referred to here does not include a dichroic dye having a polymerizable group. Hereinafter, a polymerizable liquid crystal compound other than a dichroic dye having a polymerizable group is referred to as a "polymerizable liquid crystal compound (A)". In the present invention, the composition for forming a polarizer preferably contains a liquid crystal substance having a polymerizable group, and in one embodiment of the present invention, the composition for forming a polarizer contains a polymerizable liquid crystal compound (A) as a liquid crystal substance having a polymerizable group.
[0068] Examples of the polymerizable group of the polymerizable liquid crystal compound (A) include the groups exemplified as the polymerizable group of the structural unit (ii) constituting the polymer (I') forming the photo-alignment film. Among them, from the viewpoint of easy control of the reaction, the preferred polymerizable group is a (meth)acryloyl group, a (meth)acryloyloxy group, a vinyloxy group, an oxiranyl group, and an oxetanyl group, more preferably a (meth)acryloyl group and a (meth)acryloyloxy group, and even more preferably a (meth)acryloyloxy group. The polymerizable group in the polymerizable liquid crystal compound (A) may be one type or a combination of two or more types. Since a bond can be formed between the polymerizable group of the structural unit (ii) constituting the polymer (I'), it is easy to form a polarizing film having excellent adhesion between the photo-alignment film and the polarizer, so it is preferable that the polymerizable group of the polymerizable liquid crystal compound (A) is the same polymerizable group as the polymerizable group in the structural unit (ii).
[0069] The polymerizable liquid crystal compound (A) may be a thermotropic liquid crystal or a lyotropic liquid crystal, but is preferably a thermotropic liquid crystal. The polymerizable liquid crystal compound (A) may be a thermotropic liquid crystal compound exhibiting a nematic liquid crystal phase or a thermotropic liquid crystal compound exhibiting a smectic liquid crystal phase. In the present invention, the polymerizable liquid crystal compound (A) is preferably a thermotropic liquid crystal compound exhibiting a smectic liquid crystal phase, more preferably a thermotropic liquid crystal compound exhibiting a high-order smectic liquid crystal phase, from the viewpoint of obtaining higher polarization characteristics. Among them, a thermotropic liquid crystal compound exhibiting a smectic B phase, a smectic D phase, a smectic E phase, a smectic F phase, a smectic G phase, a smectic H phase, a smectic I phase, a smectic J phase, a smectic K phase, or a smectic L phase is more preferable, and a thermotropic liquid crystal compound exhibiting a smectic B phase, a smectic F phase, or a smectic I phase is even more preferable. When the liquid crystal phase formed by the polymerizable liquid crystal compound (A) is such a high-order smectic phase, a polarizer with higher polarization performance can be obtained. In addition, such a polarizer with high polarization performance can obtain a Bragg peak derived from a high-order structure such as a hexatic phase or a crystalline phase in X-ray diffraction measurement. The polarizer of the present invention preferably contains a polymer of such a polymerizable liquid crystal compound, preferably a polymer of a polymerizable liquid crystal compound polymerized in a smectic phase state, from the viewpoint of obtaining higher polarization characteristics.
[0070] The polymerizable liquid crystal compound (A) is not particularly limited as long as it is a liquid crystal compound having at least one polymerizable group, and a known polymerizable liquid crystal compound can be used, but a compound showing smectic liquid crystallinity is preferable. For example, such a polymerizable liquid crystal compound includes a compound represented by the following formula (A1) (hereinafter, sometimes referred to as "polymerizable liquid crystal compound (A1)"). U 1A -V 1A -W 1A -(X 1A -Y 1A -) n -X 2A -W A2 -V2A -U 2A (A1) [In formula (A1), X 1A and X 2A represent, independently of each other, a divalent aromatic group or a divalent alicyclic hydrocarbon group, in which a hydrogen atom contained in the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with a halogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms, an alkoxy group having 1 to 4 carbon atoms, a cyano group, or a nitro group, and a carbon atom constituting the divalent aromatic group or the divalent alicyclic hydrocarbon group may be substituted with an oxygen atom, a sulfur atom, or a nitrogen atom. 1A and X 2A At least one of these is a 1,4-phenylene group which may have a substituent or a cyclohexane-1,4-diyl group which may have a substituent. Y 1A is a single bond or a divalent linking group. n is 1 to 3. If n is 2 or more, multiple X 1A may be the same or different. X 2A is multiple X 1A may be the same as or different from any one or all of Y. 1A may be the same or different. From the viewpoint of liquid crystallinity, n is preferably 2 or more. U 1A represents a hydrogen atom or a polymerizable group. U 2A represents a polymerizable group. W 1A and W 2A are each independently a single bond or a divalent linking group. V 1A and V 2A each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent, and -CH2- constituting the alkanediyl group may be replaced by -O-, -CO-, -S- or NH-.]
[0071] In the polymerizable liquid crystal compound (A1), X 1A and X 2A are each independently preferably an optionally substituted 1,4-phenylene group or an optionally substituted cyclohexane-1,4-diyl group; X 1A and X 2A At least one of the groups is a 1,4-phenylene group which may have a substituent, or a cyclohexane-1,4-diyl group which may have a substituent, and is preferably a trans-cyclohexane-1,4-diyl group. Examples of the optional substituent of the 1,4-phenylene group which may have a substituent, or the cyclohexane-1,4-diyl group which may have a substituent, include an alkyl group having 1 to 4 carbon atoms such as a methyl group, an ethyl group, and a butyl group, a cyano group, and a halogen atom such as a chlorine atom or a fluorine atom. It is preferably unsubstituted.
[0072] The polymerizable liquid crystal compound (A1) is a compound represented by the formula (A1-1): -(X 1A -Y 1A -) n -X 2A - (A1-1) [In the formula, X 1A , Y 1A , X 2A and n have the same meanings as above. [hereinafter, also referred to as partial structure (A1-1)] preferably has an asymmetric structure in that smectic liquid crystallinity is easily exhibited. The polymerizable liquid crystal compound (A1) in which the partial structure (A1-1) is an asymmetric structure is, for example, a compound in which n is 1 and one X 1A and X 2A and Y are different from each other. 1A A compound in which two Xs are the same structure. 1A are identical in structure to each other, and one X 2A These two X 1A A polymerizable liquid crystal compound (A1) having a structure different from that of the two X 1A Of the W1A X binds to 1A But the other X 1A and X 2A The structure is different from that of the other X 1A and X 2A Also included are polymerizable liquid crystal compounds (A1) having the same structure as each other. 1A are the same structure as each other, and three X 1A and one X 2A The polymerizable liquid crystal compound (A1) includes any one of the following three structures different from all of the other three structures.
[0073] Y 1A are -CH2CH2-, -CH2O-, -CH2CH2O-, -COO-, -OCOO-, single bond, -N=N-, -CR a =CR b -, -C≡C-, -CR a =N- or -CO-NR a - is preferred. a and R b each independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1A is more preferably -CH2CH2-, -COO- or a single bond, 1A If present, X 2A Y that binds to 1A is more preferably -CH2CH2- or -CH2O-. 1A and X 2A When all of Y are the same structure, two or more Y 1A It is preferable that there is a plurality of Y 1A When the compound has a structure of asymmetric structure, the compound tends to exhibit smectic liquid crystallinity.
[0074] U 2A is a polymerizable group. 1A is a hydrogen atom or a polymerizable group, and is preferably a polymerizable group. 1A and U 2Aare preferably both polymerizable groups, and are preferably both radically polymerizable groups. Examples of the polymerizable group include the same groups as those exemplified above as the polymerizable group possessed by the polymerizable liquid crystal compound (A). If the polymerizable group is the same as the polymerizable group in the structural unit (ii) constituting the polymer (I') that forms the photo-alignment film, this is preferred because the adhesion between the photo-alignment film and the polarizer tends to be improved. 1A and a polymerizable group represented by U 2A The polymerizable groups represented by U may be different from each other, but are preferably the same type of group. 1A and U 2A At least one of the groups is preferably a (meth)acryloyl group, and more preferably both of the groups are (meth)acryloyl groups. The polymerizable group may be in a polymerized state or an unpolymerized state, but is preferably in an unpolymerized state.
[0075] V 1A and V 2A Examples of the alkanediyl group represented by the formula (I) include a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a decane-1,10-diyl group, a tetradecane-1,14-diyl group, and an icosane-1,20-diyl group. 1A and V 2A is preferably an alkanediyl group having 2 to 12 carbon atoms, and more preferably an alkanediyl group having 6 to 12 carbon atoms.
[0076] Examples of the substituent that the alkanediyl group may have include a cyano group and a halogen atom. The alkanediyl group is preferably unsubstituted, and more preferably an unsubstituted linear alkanediyl group.
[0077] W 1A and W 2Aare each independently preferably a single bond, -O-, -S-, -COO- or -OCOO-, more preferably a single bond or -O-.
[0078] The polymerizable liquid crystal compound (A) is not particularly limited as long as it has at least one polymerizable group and exhibits liquid crystallinity, and known polymerizable liquid crystal compounds can be used. As the polymerizable liquid crystal compound (A), a polymerizable liquid crystal compound exhibiting smectic liquid crystallinity is preferred, and a compound exhibiting high-order smectic liquid crystallinity is more preferred. As a structure that is likely to exhibit smectic liquid crystallinity, it is preferred to have an asymmetric molecular structure in the molecular structure, and more specifically, it is more preferred to have a polymerizable liquid crystal compound having a structure represented by the following formulas (Aa) to (Ai) and exhibiting smectic liquid crystallinity. From the viewpoint of being likely to exhibit high-order smectic liquid crystallinity, it is more preferred to have a structure represented by any of formulas (Aa), (Ab), and (Ac), and it is particularly preferred to have a structure represented by formula (Aa) or (Ac). In the following formulas, * represents a bond.
[0079] [ka]
[0080] Specific examples of the polymerizable liquid crystal compound (A) include compounds represented by formulae (A-1) to (A-25). When the polymerizable liquid crystal compound (A) has a cyclohexane-1,4-diyl group, the cyclohexane-1,4-diyl group is preferably a trans isomer.
[0081] [ka]
[0082] [ka]
[0083] [ka]
[0084] [ka]
[0085] [ka]
[0086] Among these, at least one selected from the group consisting of compounds represented by formula (A-2), formula (A-3), formula (A-4), formula (A-5), formula (A-6), formula (A-7), formula (A-8), formula (A-13), formula (A-14), formula (A-15), formula (A-16) and formula (A-17) is preferred. As the polymerizable liquid crystal compound (A), one type may be used alone, or two or more types may be used in combination.
[0087] The polymerizable liquid crystal compound (A) can be produced by a known method, for example, as described in Lub et al., Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996), or Japanese Patent No. 4,719,156.
[0088] In the present invention, when the composition for forming a polarizer contains the polymerizable liquid crystal compound (A), the content thereof may be, for example, 1 to 99 parts by mass relative to 100 parts by mass of the solid content of the composition for forming a polarizer, and is preferably 40 parts by mass or more, more preferably 50 parts by mass or more, even more preferably 60 parts by mass or more, particularly preferably 70 parts by mass or more, and especially preferably 80 parts by mass or more, and is preferably 98 parts by mass or less, more preferably 95 parts by mass or less.
[0089] When the composition for forming a polarizer contains two or more polymerizable liquid crystal compounds (A), at least one of them may be the polymerizable liquid crystal compound (A1), or all of them may be the polymerizable liquid crystal compound (A1). By combining a plurality of polymerizable liquid crystal compounds, liquid crystallinity may be temporarily maintained even at a temperature below the liquid crystal-crystal phase transition temperature.
[0090] The polarizer-forming composition may further include a polymerization initiator. The polymerization initiator is a compound capable of initiating a polymerization reaction of a liquid crystal material having a polymerizable group that can be included in the polarizer-forming composition. The polymerization initiator is not particularly limited as long as it is a compound capable of initiating a polymerization reaction of a liquid crystal material having a polymerizable group, and a known polymerization initiator, preferably a photopolymerization initiator, can be used. Specifically, a photopolymerization initiator that generates active radicals by light irradiation or a photopolymerization initiator that generates an acid can be used. The photopolymerization initiator can be used alone or in combination of two or more kinds.
[0091] Examples of photopolymerization initiators that generate active radicals include self-cleavage type photopolymerization initiators such as benzoin compounds, acetophenone compounds, hydroxyacetophenone compounds, α-aminoacetophenone compounds, oxime ester compounds, acylphosphine oxide compounds, and azo compounds, and hydrogen abstraction type photopolymerization initiators such as benzophenone compounds, alkylphenone compounds, benzoin ether compounds, benzyl ketal compounds, dibenzosuberone compounds, anthraquinone compounds, xanthone compounds, thioxanthone compounds, halogenoacetophenone compounds, dialkoxyacetophenone compounds, halogenobisimidazole compounds, halogenotriazine compounds, and triazine compounds. Examples of photopolymerization initiators that generate an acid include iodonium salts and sulfonium salts. Among these photopolymerization initiators, photopolymerization initiators that generate active radicals upon irradiation with light are preferred, and among these, from the viewpoint of excellent reaction efficiency at low temperatures, self-cleavage type photopolymerization initiators are preferred, and in particular, acetophenone-based compounds, hydroxyacetophenone-based compounds, α-aminoacetophenone-based compounds, and oxime ester-based compounds are preferred.
[0092] Examples of the benzoin compound include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin isobutyl ether.
[0093] Examples of acetophenone compounds include diethoxyacetophenone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1,2-diphenyl-2,2-dimethoxyethane-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, and oligomers of 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one.
[0094] Examples of oxime ester compounds include Irgacure (registered trademark) OXE-01, Irgacure (registered trademark) OXE-02, Irgacure (registered trademark) OXE-03 (all manufactured by BASF Japan Ltd.), ADEKA OPTOMER (registered trademark) N-1919, ADEKA ARCLES (registered trademark) NCI-831 (all manufactured by ADEKA Corporation).
[0095] Examples of the acylphosphine oxide compound include 2,4,6-trimethylbenzoyldiphenylphosphine oxide and bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide.
[0096] Examples of the benzophenone compound include benzophenone, methyl o-benzoylbenzoate, 4-phenylbenzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, and 2,4,6-trimethylbenzophenone.
[0097] Examples of alkylphenone compounds include diethoxyacetophenone, 2-methyl-2-morpholino-1-(4-methylthiophenyl)propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)butan-1-one, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1,2-diphenyl-2,2-dimethoxyethane-1-one, 2-hydroxy-2-methyl-1-[4-(2-hydroxyethoxy)phenyl]propan-1-one, 1-hydroxycyclohexyl phenyl ketone, and oligomers of 2-hydroxy-2-methyl-1-[4-(1-methylvinyl)phenyl]propan-1-one.
[0098] Examples of the triazine compound include 2,4-bis(trichloromethyl)-6-(4-methoxyphenyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxynaphthyl)-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-(4-methoxystyryl)-1,3,5-triazine, and 2,4-bis(trichloromethyl)-6-[2-(5-methylfuran-2-yl)ethene].
[0036] 2,4-bis(trichloromethyl)-6-[2-(furan-2-yl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(4-diethylamino-2-methylphenyl)ethenyl]-1,3,5-triazine, 2,4-bis(trichloromethyl)-6-[2-(3,4-dimethoxyphenyl)ethenyl]-1,3,5-triazine, and the like.
[0099] Examples of polymerization initiators include Irgacure 907, Irgacure 184, Irgacure 651, Irgacure 819, Irgacure 250, and Irgacure 369 (all manufactured by Chiba Japan Co., Ltd.), Seikuol BZ, Seikuol Z, and Seikuol BEE (all manufactured by Seiko Chemical Co., Ltd.), Kayacure BP100 (manufactured by Nippon Kayaku Co., Ltd.), Kayacure UVI-6992 (manufactured by Dow Chemical Co., Ltd.), Adeka Optomer SP-152 or Adeka Optomer SP-170 (all manufactured by ADEKA Corporation), TAZ-A and TAZ-PP (all manufactured by Nippon SiberHegner Co., Ltd.), TAZ-104 (manufactured by Sanwa Chemical Co., Ltd.), Esacure One, and Esacure KIP 150 (all manufactured by IGM Chemical Co., Ltd.), and Commercially available photopolymerization initiators such as those manufactured by Resins can also be used.
[0100] When the polarizer-forming composition contains a polymerization initiator, the content of the polymerization initiator may be appropriately adjusted according to the type and amount of the liquid crystal substance having a polymerizable group contained in the polarizer-forming composition that is involved in the polymerization reaction. The content of the polymerization initiator is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, and even more preferably 1 to 10 parts by mass, based on 100 parts by mass of the solid content of the polarizer-forming composition.
[0101] The polarizer-forming composition may contain additives as necessary, as long as the effects of the present invention are not impaired. Examples of the additives include a sensitizer, a polymerization inhibitor, and a leveling agent.
[0102] The polarizer-forming composition may contain a sensitizer. The sensitizer is preferably a photosensitizer. Examples of the sensitizer include xanthone compounds such as xanthone or thioxanthone (e.g., 2,4-diethylthioxanthone, 2-isopropylthioxanthone, etc.), anthracene compounds having a substituent such as anthracene or alkyl ether (e.g., dibutoxyanthracene, etc.), phenothiazine, and rubrene.
[0103] When the composition for forming a polarizer contains a sensitizer, the polymerization reaction of the liquid crystal substance having a polymerizable group contained in the composition is promoted, and the film strength of the obtained polarizer is likely to be improved. When the composition for forming a polarizer contains a photosensitizer, the content of the sensitizer is preferably 0.1 to 30 parts by mass, more preferably 0.3 to 10 parts by mass, and even more preferably 0.5 to 8.0 parts by mass relative to 100 parts by mass of the solid content of the composition for forming a polarizer, from the viewpoint of easily promoting the polymerization reaction without impairing the alignment of the obtained polarizer.
[0104] Examples of the polymerization inhibitor include hydroquinone or hydroquinones having a substituent such as alkyl ether, catechols having a substituent such as alkyl ether, such as butylcatechol, pyrogallols, radical scavengers such as 2,2,6,6-tetramethyl-1-piperidinyloxy radical, thiophenols, β-naphthylamines, and β-naphthols.
[0105] When the composition for forming a polarizer contains a polymerization inhibitor, the composition can be polymerized while suppressing the occurrence of alignment disorder of the liquid crystal substance having a polymerizable group. When the composition for forming a polarizer contains a polymerization inhibitor, the content of the polymerization inhibitor is preferably 0.1 to 30 parts by mass, more preferably 0.3 to 10 parts by mass, and even more preferably 0.5 to 8.0 parts by mass relative to 100 parts by mass of the solid content of the composition for forming a polarizer, from the viewpoint of the effect of suppressing alignment disorder of the liquid crystal substance having a polymerizable group.
[0106] The polarizer-forming composition may contain a leveling agent. The leveling agent is an additive that adjusts the fluidity of the composition and makes the film obtained by applying the composition flatter, and examples of the leveling agent include organic modified silicone oil-based, polyacrylate-based, and perfluoroalkyl-based leveling agents. Specifically, DC3PA, SH7PA, DC11PA, SH28PA, SH29PA, SH30PA, ST80PA, ST86PA, SH8400, SH8700, FZ2123 (all manufactured by Dow Corning Toray Co., Ltd.), KP321, KP323, KP324, KP326, KP340, KP341, X22-161A, KF6001 (all manufactured by Shin-Etsu Chemical Co., Ltd.), TSF400, TSF401, TSF410, TSF4300, TSF4440, TSF4445, TSF-4446, TSF4452, TSF4460 (all manufactured by Momentive Performance Materials Co., Ltd.) Japan LLC), Fluorinert (registered trademark) FC-72, FC-40, FC-43, FC-3283 (all manufactured by Sumitomo 3M Limited), Megafac (registered trademark) R-08, R-30, R-90, F-410, F-411, F-443, F-445, F-470, F-477, F-479, F-482, F-483 (all manufactured by DIC Corporation), F-top (trade name) EF301, EF303, EF351, EF352 (all manufactured by Mitsubishi Materials Electronics Co., Ltd.), Surflon (registered trademark) S-381, S-382, S-383, S-393, SC-101, SC-105, KH-40, SA-100 (all manufactured by AGC Seimi Chemical Co., Ltd.), trade names E1830, E5844 (manufactured by Daikin Fine Chemical Research Institute Co., Ltd.), BM-1000, BM-1100, BYK-352, BYK-353 and BYK-361N (all trade names: manufactured by BM Chemie Co., Ltd.), etc. Among them, polyacrylate-based leveling agents and perfluoroalkyl-based leveling agents are preferred.
[0107] When the composition for forming a polarizer contains a leveling agent, the amount of the leveling agent is preferably 0.01 to 30 parts by mass, more preferably 0.03 to 10 parts by mass, and further preferably 0.05 to 8.0 parts by mass, relative to 100 parts by mass of the solid content of the composition for forming a polarizer, from the viewpoints of improving the alignment and making it easy to smooth the resulting polarizer. The leveling agents may be used alone or in combination of two or more kinds.
[0108] Further, examples of additives that the polarizer-forming composition may contain other than the sensitizer, polymerization inhibitor, and leveling agent include antioxidants, release agents, stabilizers, colorants such as bluing agents, flame retardants, and lubricants. When the polarizer-forming composition contains these additives, the total mass of the additives is preferably more than 0% and not more than 20% by mass, more preferably more than 0% and not more than 10% by mass, based on the solid content of the polarizer-forming composition.
[0109] The composition for forming a polarizer can be produced by a conventionally known preparation method, and can usually be prepared by mixing and stirring a dichroic dye, a polymerizable liquid crystal compound (A) if necessary, a polymerization initiator, the above-mentioned additives, etc. In addition, since a compound exhibiting smectic liquid crystallinity generally has high viscosity, from the viewpoint of improving the coatability of the composition for forming a polarizer and facilitating the formation of a polarizer, a solvent may be added to the composition for forming a polarizer to adjust the viscosity.
[0110] The solvent is preferably an organic solvent that can dissolve the components contained in the polarizer-forming composition and is inactive in the polymerization reaction. Specifically, for example, alcohol solvents such as methanol, ethanol, ethylene glycol, isopropyl alcohol, propylene glycol, methyl cellosolve, butyl cellosolve, or propylene glycol monomethyl ether; ester solvents such as ethyl acetate, butyl acetate, ethylene glycol methyl ether acetate, γ-butyrolactone, propylene glycol methyl ether acetate, or ethyl lactate; ketone solvents such as acetone, methyl ethyl ketone, cyclopentanone, cyclohexanone, methyl amyl ketone, or methyl isobutyl ketone; non-chlorine-based aliphatic hydrocarbon solvents such as pentane, hexane, or heptane; non-chlorine-based aromatic solvents such as toluene, xylene, or phenol, and nitrile solvents such as acetonitrile; ether solvents such as tetrahydrofuran or dimethoxyethane; chlorine-based aliphatic hydrocarbon solvents such as chloroform or chlorobenzene; amide solvents such as dimethylacetamide, dimethylformamide, N-methyl-2-pyrrolidone, and 1,3-dimethyl-2-imidazolidinone. These organic solvents may be used alone or in combination of two or more.
[0111] When the polarizer-forming composition contains a solvent, the solid content of the polarizer-forming composition is preferably 2% by mass or more, more preferably 5% by mass or more, and even more preferably 10% by mass or more, and is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less. When the solid content is at least the lower limit, the resulting polarizer does not become too thin, and the dichroism required for the polarizer is easily obtained. When the solid content is at most the upper limit, the viscosity of the polarizer-forming composition is low, and the coating film of the composition tends to be less likely to have uneven thickness.
[0112] The viscosity of the polarizer-forming composition is preferably 0.1 to 10 mPa s, more preferably 0.1 to 7 mPa s, and even more preferably 0.1 to 5 mPa s. When the viscosity of the polarizer-forming composition is within the above range, the composition has excellent handleability and coatability, and the thickness of the obtained polarizer can be easily made uniform.
[0113] In the present invention, the polarizer is a cured product of a liquid crystal composition (polarizer-forming composition), and can be obtained by polymerizing the liquid crystal substance contained in the composition. A polarizer is a device that splits non-polarized incident light into two orthogonal polarized components, transmits one polarized component, and absorbs the other polarized component. The axial direction of the transmitted polarized component is called the transmission axis, and the axial direction of the absorbed polarized component is called the absorption axis.
[0114] In the present invention, the polarizer is adjacent to the photo-alignment film, and can exhibit high adhesion with the photo-alignment film.One of the reasons for this effect is that when forming a polarizer, which is a cured product of a liquid crystal composition, the liquid crystal compound or dichroic dye having a polymerizable group for forming the polarizer reacts with the polymerizable group contained in the polymer (I') constituting the photo-alignment film, and bonds with the polymerizable group of the liquid crystal compound or dichroic dye that forms the polarizer, thereby forming a tighter bond between the polarizer and the photo-alignment film.
[0115] In addition, the photo-alignment film formed from the polymer (I') has excellent solvent resistance, and therefore exhibits high liquid crystal alignment ability, making it easy to form a polarizer with a high degree of alignment order. A polarizer with a high degree of alignment order exhibits a Bragg peak derived from a higher-order structure such as a hexatic phase or a crystalline phase in X-ray diffraction measurement. The Bragg peak means a peak derived from a planar periodic structure of molecular alignment, and the polarizer constituting the polarizing film of the present invention preferably exhibits a Bragg peak in X-ray diffraction measurement. That is, in the polarizer constituting the polarizing film of the present invention, the polymerizable liquid crystal compound or its polymer is preferably oriented so that the polarizer exhibits a Bragg peak in X-ray diffraction measurement, and more preferably has a "horizontal alignment" in which the molecules of the polymerizable liquid crystal compound are oriented in the direction in which light is absorbed. In the present invention, a polarizer in which the planar periodicity of the molecular alignment is 3.0 to 6.0 Å is preferable. A high degree of alignment order that exhibits a Bragg peak can be realized by controlling the type of polymerizable liquid crystal compound used, the type and amount of the dichroic dye, and the type and amount of the polymerization initiator.
[0116] The thickness of the polarizer can be appropriately determined depending on the use of the optical laminate in which the polarizing film is incorporated, and is preferably 0.1 μm to 10 μm, more preferably 0.3 μm to 5 μm, and even more preferably 0.5 μm to 3 μm. If the thickness of the polarizer is equal to or greater than the lower limit, the liquid crystal substance is unlikely to be aligned in the vertical direction, and the alignment order is likely to be improved. If the thickness of the polarizer is equal to or less than the upper limit, the liquid crystal substance is unlikely to be aligned randomly, and the alignment order is likely to be improved. The thickness of the polarizer can be measured using an interference thickness gauge, a laser microscope, a stylus thickness gauge, or the like.
[0117] The polarizer can be obtained, for example, by a method including applying a polarizer-forming composition onto a photo-alignment film and curing the applied polarizer-forming composition. In one embodiment of the present invention, when the polarizer-forming composition contains a solvent, a polarizer may be formed by applying the polarizer-forming composition, removing the solvent contained in the composition, and curing the polarizer-forming composition from which the solvent has been removed. Furthermore, when the composition for forming a polarizer contains a polymerizable liquid crystal compound as a liquid crystalline substance, the polarizer can be obtained, for example, by a method including raising the temperature to a temperature at which the polymerizable liquid crystal compound undergoes a phase transition to a liquid phase or higher, and then lowering the temperature to cause the polymerizable liquid crystal compound to undergo a phase transition to a liquid crystal phase (smectic phase), and polymerizing the polymerizable liquid crystal compound while maintaining the liquid crystal phase.
[0118] Examples of a method for applying the polarizer-forming composition onto a photoalignment film include known methods such as application methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography.
[0119] In the case of removing the solvent, the solvent is removed by drying or the like, preferably under conditions in which the polymerizable liquid crystal compound contained in the coating film of the polarizer-forming composition does not polymerize, to form a dried coating film. Examples of the drying method include natural drying, ventilation drying, heat drying, and reduced pressure drying.
[0120] The drying temperature may be, for example, 50 to 200°C, preferably 100°C or higher, more preferably 110°C or higher, further preferably 120°C or higher, and preferably 150°C or lower. When the drying temperature is within the above range, the solvent in the coating film can be efficiently removed. In addition, the effect of temperature on the photo-alignment film on which the coating film is formed can be suppressed, and the liquid crystal alignment ability of the photo-alignment film is less likely to decrease. The drying time is preferably 20 seconds to 10 minutes, more preferably 30 seconds to 5 minutes.
[0121] When the liquid crystalline substance is caused to undergo phase transition to a liquid phase, such phase transition may be carried out after removal of the solvent in the coating film or simultaneously with removal of the solvent.
[0122] By polymerizing the liquid crystal substance while maintaining the liquid crystal state, a polarizer is formed as a cured product of the polarizer-forming composition. The polymerization method may be appropriately selected from photopolymerization, thermal polymerization, and the like depending on the type of polymerizable group. When polymerization is performed by photopolymerization, polymerization can be performed at a low temperature, and industrial production is also easy, so in one embodiment of the present invention, photopolymerization is preferred as the polymerization method. In photopolymerization, the light irradiated to the dried coating film is appropriately selected depending on the type of polymerizable liquid crystal compound, etc. contained in the dried coating film (particularly, the type of polymerizable group possessed by the polymerizable liquid crystal compound, etc.), the type of polymerization initiator, and the amount thereof. Specific examples thereof include one or more active energy rays and active electron beams selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α-rays, β-rays, and γ-rays. Among them, ultraviolet light is preferred because it is easy to control the progress of the polymerization reaction and a photopolymerization device that is widely used in this field can be used. It is preferable to select the type of polymerizable liquid crystal compound and polymerization initiator contained in the polarizer-forming composition so that they can be photopolymerized by ultraviolet light. In addition, the polymerization temperature can be controlled by irradiating light while cooling the dried coating film with an appropriate cooling means during polymerization. During photopolymerization, a patterned polarizer can also be obtained by performing masking and development.
[0123] Examples of the light source of the active energy rays include a low pressure mercury lamp, a medium pressure mercury lamp, a high pressure mercury lamp, an ultra-high pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 380 to 440 nm, a chemical lamp, a black light lamp, a microwave excited mercury lamp, and a metal halide lamp.
[0124] The UV irradiation intensity is usually 10 to 3,000 mW / cm 2The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a polymerization initiator. The time for light irradiation is usually 0.1 seconds to 10 minutes, preferably 1 second to 5 minutes, more preferably 5 seconds to 3 minutes, and further preferably 10 seconds to 1 minute. When irradiating once or multiple times with such ultraviolet irradiation intensity, the integrated light amount is 10 to 3,000 mJ / cm. 2 , preferably 50 to 2,000 mJ / cm 2 , more preferably 100 to 1,000 mJ / cm 2 It is.
[0125] When the composition for forming a polarizer contains a polymerizable liquid crystal compound (A), the polymerizable liquid crystal compound (A) is polymerized by photopolymerization while maintaining the liquid crystal state of a liquid crystal phase, particularly a smectic phase, preferably a high-order smectic phase, to form a polarizer. The polarizer obtained by polymerizing the polymerizable liquid crystal compound while maintaining the liquid crystal state of a smectic phase has an advantage of having higher polarization performance due to the action of the dichroic dye, compared to conventional host-guest type polarizing films, i.e., polarizers made of a liquid crystal state of a nematic phase. Furthermore, it has an advantage of having superior strength compared to those coated with only a dichroic dye or a lyotropic liquid crystal.
[0126] [Polarizing Plate] The present invention also includes a polarizing plate comprising the polarizing film of the present invention and a substrate disposed on the photoalignment film side of the polarizing film.
[0127] The substrate can be, for example, glass substrate and film substrate, and film substrate is preferred.The resin that constitutes the film substrate can be, for example, polyolefin such as polyethylene, polypropylene, norbornene polymer, cyclic olefin resin, polyvinyl alcohol, polyethylene terephthalate, polymethacrylic acid ester, polyacrylic acid ester, cellulose ester such as triacetyl cellulose, diacetyl cellulose and cellulose acetate propionate, polyethylene naphthalate, polycarbonate, polysulfone, polyether sulfone, polyether ketone, polyphenylene sulfide and polyphenylene oxide.
[0128] Examples of commercially available cellulose ester substrates include "FUJITAC FILM" (manufactured by Fuji Photo Film Co., Ltd.); "KC8UX2M", "KC8UY" and "KC4UY" (all manufactured by Konica Minolta Opto, Inc.). Examples of commercially available cyclic olefin resins include "Topas" (registered trademark) (manufactured by Ticona, Germany), "Arton" (registered trademark) (manufactured by JSR Corporation), "ZEONOR" (registered trademark), "ZEONEX" (registered trademark) (all manufactured by Zeon Corporation), and "Apel" (registered trademark) (manufactured by Mitsui Chemicals, Inc.). Such cyclic olefin resins can be formed into a film by known means such as a solvent casting method or a melt extrusion method to form a substrate. Commercially available cyclic olefin resin substrates can also be used. Examples of commercially available cyclic olefin resin substrates include "S-Cina" (registered trademark), "SCA40" (registered trademark) (all manufactured by Sekisui Chemical Co., Ltd.), "ZEONOR Film" (registered trademark) (manufactured by Optes Co., Ltd.), and "Arton Film" (registered trademark) (manufactured by JSR Corporation).
[0129] The properties required for the substrate vary depending on the configuration of the polarizing plate, but generally, a substrate with as small a retardation as possible is preferred. Examples of substrates with as small a retardation as possible include cellulose ester films with no retardation, such as Zerotack (Konica Minolta Opto, Inc.) and Z-tack (Fujifilm Corporation). Unstretched cyclic olefin resin substrates are also preferred. The surface of the substrate on which the polarizing film is not laminated may be subjected to hard coat treatment, antireflection treatment, antistatic treatment, etc.
[0130] The thickness of the substrate is preferably thin from the viewpoint of practical handling, but is preferably thick from the viewpoint of strength and processability. In one embodiment of the present invention, the thickness of the substrate is preferably 5 μm to 300 μm, more preferably 20 μm to 200 μm. In addition, since it is possible to apply only the polarizing film of the present invention to an optical laminate such as an elliptical polarizing plate by peeling the polarizing film from the substrate and transferring the polarizing film, the effect of further reducing the thickness of the optical laminate used in an image display panel or the like can be obtained.
[0131] [Optical laminate] The present invention also includes an optical laminate including the polarizing plate of the present invention and a layer attached to the polarizer side of the polarizing plate via a tacky adhesive layer. In such an optical laminate, examples of the layer attached to the polarizer of the present invention include various optical layers and protective layers. Examples of the various optical layers include layers that function for image display (display screen, etc.) (for example, layers that function to improve the visibility of images) and films having various optical properties that can be incorporated into image display devices. Such optical layers may be, for example, a single-layer structure (for example, optically functional films such as retardation films, brightness-enhancing films, anti-glare films, anti-reflection films, diffusion films, and light-collecting films) or a multilayer structure (for example, a retardation plate, etc.).
[0132] In the optical laminate of the present invention, the adhesive layer for adhesively bonding the polarizer and the layer to be attached to the polarizer is a layer formed from an adhesive. As the adhesive forming the adhesive layer, any adhesive conventionally known in the art can be used depending on the type of layer to be attached to the polarizer, the layer configuration of the optical laminate, and the like. The thickness of the adhesive layer may be appropriately determined depending on the layer structure of the optical laminate, and may be, for example, 0.1 to 30 μm.
[0133] The present invention also includes an elliptical polarizing plate comprising the polarizing film of the present invention and a retardation layer having a ¼ wavelength plate function (hereinafter also referred to as a “λ / 4 retardation layer”). The (elliptical) circular polarizing plate is a functional layer having a function of transmitting only right- or left-handed circularly polarized light components by laminating a λ / 4 retardation plate on a linear polarizing plate. The elliptical polarizing plate of the present invention may have a λ / 4 retardation layer on either one side of the polarizing film of the present invention.
[0134] The λ / 4 retardation layer constituting the elliptically polarizing plate of the present invention preferably satisfies the optical properties represented by the following formulas (a), (b) and (c). Re(450) / Re(550)≦1.00 (a) 1.00≦Re(650) / Re(550) (b) 120≦Re(550)≦180 (c) (In the formula, Re(λ) represents an in-plane retardation value of the retardation layer at a wavelength of λ nm, and Re=(nx(λ)-ny(λ))×d (d represents the thickness of the retardation layer, nx represents the principal refractive index at a wavelength of λ nm in a direction parallel to the plane of the retardation layer in the index ellipsoid formed by the retardation layer, and ny represents the refractive index at a wavelength of λ nm in a direction parallel to the plane of the retardation layer and perpendicular to the direction of nx in the index ellipsoid formed by the retardation layer).)
[0135] When the retardation layer satisfies the formulas (a) and (b), the retardation layer exhibits the so-called reverse wavelength dispersion, in which the in-plane retardation value at a short wavelength is smaller than the in-plane retardation value at a long wavelength. Since the reverse wavelength dispersion is improved and the optical properties are more likely to be improved when the retardation layer is incorporated into an image display device or the like, Re(450) / Re(550) is preferably 0.70 or more, more preferably 0.78 or more, and also preferably 0.92 or less, more preferably 0.90 or less, even more preferably 0.87 or less, particularly preferably 0.86 or less, and even more particularly preferably 0.85 or less. In addition, Re(650) / Re(550) is preferably 1.0 or more, more preferably 1.01 or more, and even more preferably 1.02 or more.
[0136] The retardation layer may be a stretched film that imparts retardation by stretching a polymer, or a liquid crystal cured layer made of a cured liquid crystal composition containing a polymerizable liquid crystal compound. These λ / 4 retardation layers can be produced by appropriately selecting and adopting materials and methods conventionally known in the art.
[0137] The thickness of the λ / 4 retardation layer is not particularly limited and may be, for example, 100 μm or less, and is preferably 0.5 μm to 20 μm, more preferably 1 μm to 3 μm, from the viewpoint of thinning the image display device in which it is incorporated. A very thin retardation layer having a thickness of 1 μm to 3 μm can be produced by using a liquid crystal cured layer obtained by curing a polymerizable liquid crystal compound in an aligned state.
[0138] When laminating the polarizing film of the present invention and the λ / 4 retardation layer, it is preferable to laminate them so that the slow axis (optical axis) of the λ / 4 retardation layer and the absorption axis of the polarizer are substantially 45°. By laminating them so that the slow axis (optical axis) of the retardation layer and the absorption axis of the polarizer are substantially 45°, it is possible to obtain the function of an elliptical polarizing plate. Note that substantially 45° is usually in the range of 45±5°.
[0139] The elliptically polarizing plate of the present invention may have a structure similar to that of a conventional general elliptically polarizing plate and / or retardation film. Examples of such structures include an adhesive layer (sheet) for attaching the elliptically polarizing plate to a display element of an optical display, a protective film used for protecting the surface of a polarizer or a retardation layer from scratches or dirt, and the like.
[0140] The elliptically polarizing plate of the present invention can be used in various display devices. The display device is a device having a display element, and includes a light-emitting element or a light-emitting device as a light source. Examples of the display device include a liquid crystal display device, an organic electroluminescence (EL) display device, an inorganic electroluminescence (EL) display device, a flexible image display device, a touch panel display device, an electron emission display device (e.g., a field emission display device (FED) and a surface field emission display device (SED)), an electronic paper (a display device using electronic ink or an electrophoretic element, a plasma display device, a projection display device (e.g., a grating light valve (GLV) display device, a display device having a digital micromirror device (DMD)), and a piezoelectric ceramic display. The liquid crystal display device includes any of a transmissive liquid crystal display device, a semi-transmissive liquid crystal display device, a reflective liquid crystal display device, a direct-view liquid crystal display device, and a projection liquid crystal display device. These display devices may be display devices that display two-dimensional images, or may be stereoscopic display devices that display three-dimensional images. In particular, the elliptical polarizing plate of the present invention can be suitably used for an organic electroluminescence (EL) display device.
[0141] In one embodiment of the present invention, the display device is preferably a flexible image display device, and the present invention also encompasses a flexible image display device comprising the elliptically polarizing plate of the present invention.
[0142] The flexible image display device having the elliptically polarizing plate of the present invention preferably further has a window and a touch sensor. A flexible image display device is, for example, composed of a laminate for a flexible image display device and an organic EL display panel, and the laminate for a flexible image display device is disposed on the viewing side of the organic EL display panel and is configured to be foldable. The laminate for a flexible image display device may include a window, a (touch panel) touch sensor, and the like in addition to the above-mentioned elliptically polarizing plate of the present invention. The order of lamination of these components is arbitrary, but it is preferable that they are laminated in the order of window, elliptically polarizing plate, and touch sensor, or the order of window, touch sensor, and elliptically polarizing plate from the viewing side.
[0143] It is preferable that an elliptically polarizing plate is present on the visible side of the touch sensor, since the pattern of the touch sensor is less visible and the visibility of the displayed image is improved. Each member can be laminated using an adhesive, a pressure sensitive adhesive, etc. In addition, the laminate for a flexible image display device can include a light shielding pattern formed on at least one surface of any one of the layers of the window, the elliptically polarizing plate, and the touch sensor.
[0144] The window is disposed on the viewing side of the flexible image display device and serves to protect other components from external impacts or environmental changes such as temperature and humidity. Conventionally, glass has been used as such a protective layer, but the window in the flexible image display device is not rigid like glass and has flexible properties. The window is made of a flexible transparent substrate and may include a hard coat layer on at least one surface.
[0145] The window, touch sensor, and the like constituting the laminate for a flexible image display device are not particularly limited, and conventionally known ones can be adopted. EXAMPLES
[0146] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. In the examples, "%" and "parts" mean mass% and mass parts, respectively, unless otherwise specified.
[0147] 1. Example 1 (1) Preparation of composition for forming photoalignment film Copolymer (1) was prepared according to the following procedure. Copolymer (1) [ka]
[0148] Chlorodimethyl ether was added dropwise to a solution prepared by dissolving 4-((6-(methacryloyloxy)hexyl)oxy)benzoic acid in toluene together with an amine catalyst, and the reaction was allowed to proceed by heating and maintaining the temperature at 40°C. Thereafter, the reaction solution was cooled and water was added. A 50% aqueous solution of acetic acid was added to the separated organic layer and stirred. The separated organic layer was concentrated to obtain methoxymethyl 4-((6-(methacryloyloxy)hexyl)oxy)benzoate. Methoxymethyl 4-((6-(methacryloyloxy)hexyl)oxy)benzoate 8.8g (25.2mmol), 6-(4-hydroxyphenoxy)hexyl methacrylate 1.0g (3.6mmol), 4-((6-(methacryloyloxy)hexyl)oxy)phenyl (E)-3-(4-methoxyphenyl)acrylate 3.2g (7.2mmol) and 2,2'-azobis(2,4-dimethylvaleronitrile) 0.2g were dissolved in tetrahydrofuran. After nitrogen was passed through the solution for 1 hour, the reaction was allowed to proceed by heating and maintaining it at 60°C, and the reaction solution was cooled to room temperature. To this reaction solution, 4-((6-(methacryloyloxy)hexyl)oxy)benzoic acid 1.1g (3.6mmol) and 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride were added to obtain a mixed solution. The reaction was allowed to proceed by heating the mixture to 40°C, and then the reaction solution was cooled. Methanesulfonic acid was added to the reaction solution at room temperature, and the reaction solution was heated to 70°C, and then cooled to around room temperature. The cooled reaction solution was dropped into normal hexane to generate a precipitate, which was then collected and dried under reduced pressure to obtain a polymer. The weight average molecular weight of the copolymer (1) was measured by GPC. The results are shown in Table 1.
[0149] In addition, 4-((6-(methacryloyloxy)hexyl)oxy)phenyl(E)-3-(4-methoxyphenyl)acrylate (a monomer that derives the photoreactive group-containing structural unit (i)) and 4-((6-(methacryloyloxy)hexyl)oxy)benzoic acid (a monomer that derives the carboxy group-containing structural unit (iii)) were prepared by the following procedure.
[0150] Monomer that derives the photoreactive group-containing structural unit (i): 4-((6-(methacryloyloxy)hexyl)oxy)phenyl (E)-3-(4-methoxyphenyl)acrylate [ka] 6-(4-hydroxyphenoxy)-1-bromohexane was synthesized by heating 1,4-dihydroxybenzene and 1,6-dibromohexane under alkaline conditions. This product was reacted with lithium methacrylate to synthesize 6-(4-hydroxyphenoxy)hexyl methacrylate. To this was added p-methoxycinnamic acid chloride under basic conditions to synthesize 4-((6-(methacryloyloxy)hexyl)oxy)phenyl (E)-3-(4-methoxyphenyl)acrylate.
[0151] Monomer from which the carboxyl group-containing structural unit (iii) is derived: 4-((6-(methacryloyloxy)hexyl)oxy)benzoic acid [ka] The compound was synthesized using methacrylic acid chloride as a raw material according to the method described in Makromol. Chem., 190, pp. 2255-2268, 1989.
[0152] Next, 2 parts of the obtained copolymer (1) and 98 parts of o-xylene were mixed, and the mixture was stirred at 80° C. for 1 hour to obtain a composition for forming a photoalignment film.
[0153] (2) Preparation of a composition for forming a polarizer A composition for forming a polarizer was obtained by mixing the following components and stirring for 1 hour at 80° C. The azo-based dye described in the examples of JP-A-2013-101328 was used as the dichroic dye. 75 parts of a polymerizable liquid crystal compound represented by formula (A-6) [ka]
[0154] 25 parts of a polymerizable liquid crystal compound represented by formula (A-7) [ka]
[0155] 2.8 parts of the dichroic dye (1) shown below [ka]
[0156] 2.8 parts of the dichroic dye (2) shown below [ka]
[0157] 2.8 parts of the dichroic dye (3) shown below [ka]
[0158] Polymerization initiator: 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; manufactured by Ciba Specialty Chemicals) 6 parts Leveling agent: Polyacrylate compound (BYK-361N; manufactured by BYK-Chemie) 1.2 parts Solvent: Cyclopentanone 250 parts
[0159] (3) Preparation of polarizing plates A triacetyl cellulose film (KC4UY-TAC manufactured by Konica Minolta, 40 μm thick) was cut into a square shape as a substrate, and treated once using a corona treatment device (AGF-B10 manufactured by Kasuga Electric Co., Ltd.) under conditions of an output of 0.3 kW and a treatment speed of 3 m / min. The composition for forming a photoalignment film was applied to the corona-treated surface using a bar coater, dried at 80° C. for 1 minute, and irradiated with 100 mJ / cm using a polarized UV irradiation device (SPOT CURE SP-7 with polarizer unit manufactured by Ushio Inc.). 2A photo-alignment film was formed by exposing the film to polarized UV light with an integrated light amount of 100 nm. The thickness of the photo-alignment film was measured with an ellipsometer M-220 (manufactured by JASCO Corporation) and found to be 100 nm.
[0160] A polarizer-forming composition was applied onto the obtained photoalignment film using a bar coater, and then dried in a drying oven set at 100° C. for 1 minute.
[0161] Thereafter, ultraviolet light was irradiated using a high-pressure mercury lamp (Uniquer VB-15201BY-A, manufactured by Ushio Electric Co., Ltd.) (under a nitrogen atmosphere, wavelength: 365 nm, cumulative light intensity at wavelength 365 nm: 1000 mJ / cm 2 ) to form a polarizer in which the polymerizable liquid crystal compound and the dichroic dye were aligned, and a polarizing plate (1) consisting of a substrate / photo-alignment film / polarizer was obtained. At this time, the thickness of the polarizer was measured by an ellipsometer and found to be 1.0 μm.
[0162] (4) Characterization [Adhesion evaluation] The adhesion between the polarizer and the photo-alignment film in the obtained polarizing plate (1) was evaluated by the following method.
[0163] (Cross-hatch test) The adhesion between the photo-alignment film and the polarizer in the obtained polarizing plate (1) was evaluated by a cross-hatch test in accordance with JIS D0202-1988 (JIS "checkerboard adhesion test"). The polarizer surface of the polarizing plate (1) was scratched in a 10 x 10 checkerboard pattern at 2 mm intervals, penetrating through to the polarizer and the photo-alignment film, to create a checkerboard pattern. An adhesive tape (25 mm wide, manufactured by Nichiban) was completely attached to the checkerboard surface. The adhesive tape was then peeled off in a direction at 90° to the surface.
[0164] The number of squares that remained unpeeled was counted and the adhesion was evaluated according to the following criteria. For the peeled squares, X-ray photoelectron spectroscopy (XPS) was used to confirm that the peeled interface was between the photo-alignment film and the polarizer. The results are shown in Table 1. <Evaluation criteria> 〇: 90 or more pieces △: 80 or more and 89 or less ×: 79 or less
[0165] [Evaluation of orientation] The obtained polarizing plate (1) was arranged in a cross-Nicol configuration through the polarizing plate from the backlight, and the orientation state of the polarizer was visually confirmed and the orientation was evaluated according to the following criteria. In addition, samples were separately prepared by drying the polarizer-forming composition for 1 minute in a drying oven set at a drying temperature of 110°C or 120°C in the same manner, and evaluated. The results are shown in Table 1. <Evaluation criteria> ◯: No disturbance in orientation ×: The orientation is disordered or there is no orientation.
[0166] 2. Examples 2 to 7 and Comparative Example 1 Polarizing plates were prepared in the same manner as in Example 1, except that the composition of the copolymer forming the photo-alignment film was changed as shown in Table 1, and the adhesion and alignment properties were evaluated. The results are shown in Table 1. The photoreactive group-containing structural unit (i), the polymerizable group-containing structural unit (ii), and the carboxy group-containing structural unit (iii) each have a structure derived from the following structure. Photoreactive group-containing structural unit (i) [ka] Polymerizable group-containing structural unit (ii) [ka] Carboxy group-containing structural unit (iii) [ka]
[0167] [Table 1]
[0168] As shown in Table 1, it was confirmed that the polarizing plates obtained in Examples 1 to 7 had high adhesion between the polarizer and the photo-alignment film. In contrast, the adhesion between the polarizer and the photo-alignment film of the polarizing plate obtained in Comparative Example 1 was insufficient.
Claims
1. A polarizing film including a photo-alignment film and a polarizer adjacent to the photo-alignment film, the photoalignment film is formed from a polymer including a structural unit having a photoreactive group and a structural unit having a polymerizable group, The polymer forming the photoalignment film is represented by the formula (II): [In formula (II), Ma, Mb and Mc represent monomer units forming the backbone of the copolymer; m, n, and l represent mole fractions of the copolymer, with 0<m<1 and 0<n<1 and 0<l<1 in each case; SPCRa, SPCRb, and SPCRc each independently represent a spacer unit; Ring A, ring B and ring C are each independently an unsubstituted or substituted alicyclic hydrocarbon or an unsubstituted or substituted aromatic ring; X is a single covalent bond, an alkylene chain having 1 to 10 carbon atoms, or a cycloalkylene chain having 3 to 8 carbon atoms; Y is -O-CO-CH=CH 2 - (either bond may be bonded to ring B), or -N=N-; Z is selected from the group consisting of a single covalent bond; an alkylene chain having 1 to 10 carbon atoms which is unsubstituted or substituted with a hydroxyl group and / or a carbonyl group; a cycloalkylene chain having 3 to 8 carbon atoms; -O-; -COO-; and combinations thereof; R 1 is a phenyl group having at least one substituent selected from an alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a cyano group, and a halogen atom; R 2 is -CW=CH 2 or -V-CW=CH 2 (wherein W is a hydrogen atom or a methyl group, and V is -O-CO- or -CO-). The repeating unit has the following structure: The weight average molecular weight of the polymer forming the photoalignment film is 50,000 or more and 150,000 or less, The polarizer comprises a liquid crystal compound and a dichroic dye, and is a cured product of a liquid crystal composition containing a structural unit having a polymerizable group derived from the liquid crystal compound or the dichroic dye.
2. 2. The polarizing film according to claim 1, wherein the photoreactive group is a group that undergoes a dimerization reaction or an isomerization reaction.
3. 3. The polarizing film according to claim 1, wherein the dichroic dye comprises an azo dye.
4. 4. The polarizing film according to claim 1, wherein the polarizer comprises a polymer of a polymerizable liquid crystal compound.
5. 5. The polarizing film according to claim 1, wherein the polarizer exhibits a Bragg peak in X-ray diffraction measurement.
6. 6. A polarizing plate comprising the polarizing film according to claim 1 and a substrate disposed on the photo-alignment film side of the polarizing film.
7. 7. An optical laminate comprising the polarizing plate according to claim 6 and a layer attached to a polarizer side of the polarizing plate via a pressure-sensitive adhesive layer.
8. 6. An elliptically polarizing plate comprising the polarizing film according to claim 1 and a retardation layer having a quarter-wave plate function.
9. An organic electroluminescence display device comprising the elliptically polarizing plate according to claim 8 .
10. A flexible image display comprising the elliptically polarizing plate according to claim 8.
11. The flexible visual display device of claim 10 further comprising a window and a touch sensor.
Citation Information
Patent Citations
Composite method of liquid crystal supermolecule material containing double photosensitive units
CN101935368A
Retardation plate material, polymer, retardation plate, and image display apparatus
JP2005326439A
Polarization element, circularly polarizing plate and method of manufacturing those
JP2013033249A