Compositions for odor control for post-consumer resins

A blend of metal oxides and acidic copolymers with PCR enhances odor control in olefinic polymers, addressing film defects and mechanical issues, achieving significant odor reduction without compromising processability or properties.

JP7576558B2Active Publication Date: 2024-10-31DOW GLOBAL TECHNOLOGIES LLC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021549814
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-02-27
Filing Date
2020-02-18
Publication Date
2024-10-31
Estimated Expiration
2040-02-18

AI Technical Summary

Technical Problem

Existing methods for incorporating calcium oxide (CaO) into olefinic polymer articles for odor control face limitations due to high loading causing film defects, haze, color deterioration, and mechanical property degradation, while maintaining processability and desired properties.

Method used

A composition comprising 0.15% to 15% by weight of a metal oxide with a bandgap greater than 5.0 eV, such as calcium oxide, and 0.1% to 13% by weight of an acidic copolymer, is added to a polymeric component including post-consumer resin (PCR) to form an odor-reducing blend, with a metal oxide to acidic copolymer ratio of 1:20 to 1:1, enhancing odor control without compromising processability and mechanical properties.

Benefits of technology

The composition achieves at least a 20% reduction in volatile hetero-carbonyl species, maintaining film transparency and mechanical strength, and ensuring effective odor suppression in applications like vehicle interiors and food packaging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576558000001
    Figure 0007576558000001
  • Figure 0007576558000002
    Figure 0007576558000002
  • Figure 0007576558000003
    Figure 0007576558000003
Patent Text Reader

Abstract

The present disclosure provides a composition. In one embodiment, the composition includes a polymer component and an odor-inhibiting agent. The polymer component includes (i) a post-consumer resin and (ii) an optional olefin-based polymer. The composition further includes 0.15% to 15% by weight of the odor-inhibiting agent. The odor-inhibiting agent includes (i) 0.05% to 2% by weight of a metal oxide having a band gap greater than 5.0 electron volts (eV), and (ii) 0.1% to 13% by weight of an acidic copolymer. The ratio of the metal oxide to the acidic copolymer is 1:20 to 1:1. The weight percentages are based on the total weight of the composition.
Need to check novelty before this filing date? Find Prior Art

Description

[Background technology]

[0001] The environmental hazards posed by plastic waste are well known. Large-scale societal efforts have been adopted to reclaim and reuse plastic materials, commonly known as post consumer resin (PCR). Efforts to reprocess and reincorporate PCR into usable consumer goods continue to grow.

[0002] The original waste aspect of PCR means that it suffers from odor hazards and can contribute to unpleasant tastes when in contact with food. Common sources of unpleasant taste and odor include volatile hetero-carbonyl species and other chemicals inherent in PCR. There are many applications where it is desirable to blend PCR with virgin plastics. These applications require the suppression of odors from PCR as they are commercially available.

[0003] Metal oxides such as calcium oxide (CaO) are known to consume many taste and odor generating molecules. All other factors being equal, CaO concentration and odor control are known to be directly related, i.e., as CaO concentration increases in a given olefin-based polymer article, the effectiveness of odor control also increases. Similarly, as the relative surface area of ​​an adsorbent system increases, its activity and performance are also known to increase.

[0004] Although odor control increases with increasing CaO, there are limitations to the amount of CaO that can be effectively incorporated into olefin-based polymer articles. For example, in the production of blown films, high CaO particle loadings increase extrusion die lip deposition, thereby causing film defects. High CaO particle loadings also increase haze, resulting in poorer transparency of the olefin-based polymer film and / or poor color of the film. High CaO particle loadings also adversely affect mechanical properties such as impact strength and film tear strength. Processing parameters and mechanical requirements of end-use applications impose practical limitations on the loading of CaO particles into olefin-based polymer compositions. Summary of the Invention [Problem to be solved by the invention]

[0005] Thus, there is a need for PCR-containing compositions that have improved odor control while simultaneously carrying a suitable metal oxide (i.e., calcium oxide) loading to maintain end-use processability, desired optical properties, and desired mechanical properties. There is also a need for odor-controlled articles made from such PCR-containing polymer compositions.

[0006] The present disclosure provides a composition. In one embodiment, the composition includes a polymer component and an odor control agent. The polymer component includes (i) a post-consumer resin and (ii) an optional olefin-based polymer. The composition further includes 0.15% to 15% by weight of an odor control agent. The odor control agent includes (i) 0.05% to 2% by weight of a metal oxide having a band gap greater than 5.0 electron volts (eV), and (ii) 0.1% to 13% by weight of an acidic copolymer. The ratio of the metal oxide to the acidic copolymer is 1:20 to 1:1. The weight percentages are based on the total weight of the composition.

[0007] The present disclosure provides a process. In one embodiment, the process includes providing a polymer component comprised of (i) a post-consumer resin (PCR) and (ii) optionally an olefin-based polymer. The polymer component has an amount of at least one volatile hetero-carbonyl species. The process includes adding 0.15% to 15% by weight of an odor-inhibiting agent to the polymer component. The odor-inhibiting agent includes (i) 0.05% to 2% by weight of a metal oxide having a band gap greater than 5.0 electron volts (eV), and (ii) 0.1% to 13% by weight of an acidic copolymer. The ratio of the metal oxide to the acidic copolymer is 1:20 to 1:1. The process includes neutralizing at least some of the volatile hetero-carbonyl species in the PCR with the odor-inhibiting agent to form an odor-reducing composition. The weight percentage is based on the total weight of the odor-reducing composition.

[0008] definition Any reference to the Periodic Table of the Elements is to the version published by CRC Press, Inc., 1990-1991. References to element groups in this table are by the new notation for numbering groups.

[0009] For purposes of United States patent practice, the contents of any referenced patent, patent application, or publication are incorporated by reference in their entirety (or the equivalent United States version thereof is so incorporated by reference), particularly with respect to the disclosure of definitions (to the extent not inconsistent with any definitions specifically provided in this disclosure) and general knowledge in the art.

[0010] Numerical ranges disclosed herein include all values ​​from the lower limit to the upper limit, inclusive. For ranges containing explicit numbers (e.g., 1 or 2, or 3-5, or 6, or 7), any subrange between any two explicit numbers is included (e.g., 1-2, 2-6, 5-7, 3-7, 5-6, etc.).

[0011] Unless stated to the contrary, implicit from the context, or customary in the art, all parts and percentages are by weight and all testing methods are current as of the filing date of this disclosure.

[0012] The term "blend" or "polymer blend" as used herein is a blend of two or more polymers. Such blends may or may not be miscible (not phase separated at the molecular level). Such blends may or may not be phase separated. Such blends may or may not contain one or more domain configurations as determined from transmission electron spectroscopy, light scattering, x-ray scattering, and other methods known in the art.

[0013] The term "composition" refers to a mixture of materials that comprise the composition, as well as reaction products and decomposition products formed from the materials of the composition.

[0014] The terms "comprising," "including," "having," and their derivatives are not intended to exclude the presence of any additional components, steps, or procedures, whether or not they are specifically disclosed. For the avoidance of doubt, all compositions claimed through the use of the term "comprising" may include any additional additives, adjuvants, or compounds, whether polymeric or not, unless stated to the contrary. In contrast, the term "consisting essentially of" excludes any other component, step, or procedure from the scope of any succeeding description, except those that are not essential to operability. The term "consisting of" also excludes any component, step, or procedure not specifically delineated or listed. The term "or" refers to the listed members individually as well as in any combination, unless otherwise stated. The use of the singular includes the use of the plural, and vice versa.

[0015] An "ethylene-based polymer" is a polymer that contains greater than 50 weight percent (wt%) polymerized ethylene monomer (based on the total amount of polymerizable monomers) and may optionally contain at least one comonomer. Ethylene-based polymers include ethylene homopolymers and ethylene copolymers (meaning units derived from ethylene and one or more comonomers). The terms "ethylene-based polymer" and "polyethylene" may be used interchangeably. Non-limiting examples of ethylene-based polymers (polyethylenes) include low density polyethylene (LDPE) and linear polyethylene. Non-limiting examples of linear polyethylene include linear low density polyethylene (LLDPE), very low density polyethylene (ULDPE), very low density polyethylene (VLDPE), multicomponent ethylene-based copolymers (EPE), ethylene / α-olefin multiblock copolymers (also known as olefin block copolymers (OBC)), substantially linear or linear plastomers / elastomers, and high density polyethylene (HDPE). Generally, polyethylene can be produced in gas phase fluidized bed reactors, liquid phase slurry process reactors, or liquid phase solution process reactors using heterogeneous catalyst systems such as Ziegler-Natta catalysts, homogeneous catalyst systems including Group 4 transition metals and ligand structures such as metallocene, nonmetallocene metal centers, heteroaryl, heteroatom aryloxy ethers, phosphinimines, etc. Combinations of heterogeneous and / or homogeneous catalysts can also be used in either single reactor or dual reactor configurations.

[0016] "Ethylene plastomer / elastomer" refers to a polymer that contains units derived from ethylene and at least one C3-C 10It is a substantially linear or linear ethylene / α-olefin copolymer containing a uniform distribution of short chain branches including units derived from an α-olefin comonomer. The ethylene plastomer / elastomer has a density of 0.870 g / cc to 0.917 g / cc. Non-limiting examples of ethylene plastomer / elastomer include AFFINITY™ plastomers and elastomers (commercially available from Dow Chemical Company), EXACT™ plastomers (commercially available from ExxonMobil Chemical), Tafmer™ (commercially available from Mitsui), Nexlene™ (commercially available from SK Chemicals Co.), and Lucene™ (commercially available from LG Chem Ltd.).

[0017] "High density polyethylene" (or "HDPE") is a polymer consisting of ethylene homopolymer or at least one C4 to C6 10 An ethylene / α-olefin copolymer with an α-olefin comonomer or a C4-C8 α-olefin comonomer and a density of 0.940 g / cc, or 0.945 g / cc, or 0.950 g / cc, or 0.953 g / cc to 0.955 g / cc, or 0.960 g / cc, or 0.965 g / cc, or 0.970 g / cc, or 0.975 g / cc, or 0.980 g / cc. HDPE can be a unimodal or multimodal copolymer. A "unimodal ethylene copolymer" is an ethylene / C4-C8 copolymer having one distinct peak in gel permeation chromatography (GPC) showing the molecular weight distribution. 10 It is an α-olefin copolymer. A "multimodal ethylene copolymer" is an ethylene / C4-C copolymer that has at least two clear peaks in the GPC showing the molecular weight distribution. 10It is an α-olefin copolymer. Multimodal includes copolymers with two peaks (bimodal) as well as copolymers with three or more peaks. Non-limiting examples of HDPE include DOW™ high density polyethylene (HDPE) resins (commercially available from Dow Chemical Company), ELITE™ reinforced polyethylene resins (commercially available from Dow Chemical Company), CONTINUUM™ bimodal polyethylene resins (commercially available from Dow Chemical Company), LUPOLEN™ (commercially available from LyondellBasell), and HDPE products from Borealis, Ineos, and ExxonMobil.

[0018] "Interpolymers" are polymers prepared by the polymerization of at least two different monomers. This general term includes copolymers, which are commonly used to refer to polymers prepared from two different monomers, and polymers prepared from three or more different monomers, e.g., terpolymers, tetrapolymers, etc.

[0019] "Linear low density polyethylene" (or "LLDPE") is a polyethylene that is a polymer that is made up of units derived from ethylene and at least one C3-C 10 A linear ethylene / α-olefin copolymer containing a heterogeneous distribution of short chain branches including units derived from an α-olefin or a C4-C8 α-olefin comonomer. LLDPE is characterized by little, if any, long chain branching, in contrast to conventional LDPE. LLDPE has a density of less than 0.910 g / cc to 0.940 g / cc. Non-limiting examples of LLDPE include TUFLIN™ linear low density polyethylene resins (available from The Dow Chemical Company), DOWLEX™ polyethylene resins (available from The Dow Chemical Company), and MARLEX™ polyethylene (available from Chevron Phillips).

[0020] "Low density polyethylene" (or "LDPE") refers to ethylene homopolymer or at least one C3-C6 copolymer having a density between 0.915 g / cc and 0.940 g / cc and containing long chain branches with a broad MWD. 10 It consists of ethylene / α-olefin copolymers, containing α-olefins or C4-C8 α-olefins. LDPE is typically produced by high pressure free radical polymerization (tubular reactor or autoclave using a free radical initiator). Non-limiting examples of LDPE include MarFlex™ (Chevron Phillips), LUPOLEN™ (LyondellBasell), as well as LDPE products from Borealis, Ineos, ExxonMobil, etc.

[0021] “Multicomponent ethylene-based copolymers” (or “EPEs”) are copolymers that contain units derived from ethylene and at least one C3-C6 copolymer, such as those described in U.S. Pat. No. 6,111,023, U.S. Pat. No. 5,677,383, and U.S. Pat. No. 6,984,695. 10 The EPE resins include units derived from an α-olefin, or a 4 to C8 α-olefin comonomer. The EPE resins have a density of 0.905 g / cc to 0.962 g / cc. Non-limiting examples of EPE resins include ELITE™ reinforced polyethylene (commercially available from Dow Chemical Company), ELITE AT™ advanced technology resins (commercially available from Dow Chemical Company), SURPASS™ polyethylene (PE) resins (commercially available from Nova Chemicals), and SMART™ (commercially available from SK Chemicals Co.).

[0022] An "olefin-based polymer" or "polyolefin" is a polymer that contains more than 50 weight percent polymerized olefin monomers (based on the total amount of polymerizable monomers) and, optionally, may include at least one comonomer. Non-limiting examples of olefin-based polymers include ethylene-based polymers or propylene-based polymers.

[0023] A "polymer" is a compound prepared by polymerizing monomers, whether of the same or different types, that provide multiple and / or repeating "units" or "mer units" that, in polymerized form, make up the polymer. Thus, the generic term polymer encompasses the term homopolymer, which is commonly used to refer to a polymer prepared from only one type of monomer, and the term copolymer, which is commonly used to refer to a polymer prepared from at least two types of monomer. It also encompasses all forms of copolymers, e.g., random, block, etc. The terms "ethylene / α-olefin polymer" and "propylene / α-olefin polymer" refer to the above-mentioned copolymers prepared from polymerizing ethylene or propylene, respectively, with one or more additional polymerizable α-olefin monomers. It is noted that while polymers are often referred to as "made of" one or more particular monomers, "based on" a particular monomer or monomer type, "containing" a particular monomer content, etc., in this context, the term "monomer" is understood to refer to the polymerized residue of a particular monomer, and not to the non-polymerized species. Generally, polymers herein are referred to in terms of "units" that are the polymerized form of the corresponding monomers.

[0024] A "propylene-based polymer" is a polymer that contains more than 50 weight percent polymerized propylene monomer (based on the total amount of polymerizable monomers) and may optionally include at least one comonomer. Propylene-based polymers include propylene homopolymers and propylene copolymers (meaning units derived from propylene and one or more comonomers). The terms "propylene-based polymer" and "polypropylene" may be used interchangeably. Non-limiting examples of suitable propylene copolymers include propylene impact copolymers and propylene random copolymers.

[0025] "Ultra-low density polyethylene" (or "ULDPE"), and "very low density polyethylene" (or "VLDPE"), each contain units derived from ethylene and at least one C3-C 10 They are linear ethylene / α-olefin copolymers containing a heterogeneous distribution of short chain branches including units derived from the α-olefin comonomer. ULDPE and VLDPE each have a density of 0.885 g / cc to 0.915 g / cc. Non-limiting examples of ULDPE and VLDPE include ATTANE™ ultra-low density polyethylene resins (available from Dow Chemical Company) and FLEXOMER™ very low density polyethylene resins (available from Dow Chemical Company).

[0026] Test Method D10, D50, and D90 particle sizes are measured using a Coulter LS 230 laser light scattering particle sizer available from Coulter Corporation. The D10 particle size is the particle size at which 10% of the powder's mass consists of particles with a diameter less than this value. The D50 particle size is the particle size at which 50% of the powder's mass consists of particles with a diameter less than this value and 50% of the powder's mass consists of particles with a diameter greater than this value. The D90 particle size is the particle size at which 90% of the powder's mass consists of particles with a diameter less than this value. The mean volume average particle size is measured using a Coulter LS 230 laser light scattering particle sizer available from Coulter Corporation. The particle size distribution is calculated according to Equation A.

number

[0027] Density is measured according to ASTM D792, Method B. Results are reported in grams per cubic centimeter (g / cc).

[0028] Differential Scanning Calorimetry (DSC). Differential Scanning Calorimetry (DSC) can be used to measure the melting, crystallization, and glass transition behavior of polymers over a wide range of temperatures. For example, a TA Instruments Q1000 DSC equipped with an RCS (refrigerated cooling system) and an autosampler is used to perform this analysis. A nitrogen purge gas flow rate of 50 ml / min is used during testing. Each sample is melt pressed into a thin film at approximately 175°C, and the molten sample is then air cooled to room temperature (approximately 25°C). A 3-10 mg, 6 mm diameter specimen is extracted from the cooled polymer, weighed, placed in a light aluminum pan (approximately 50 mg) and crimped shut. Analysis is then performed to determine its thermal properties.

[0029] The thermal behavior of the sample is determined by ramping the sample temperature to generate a heat flow vs. temperature profile. First, the sample is rapidly heated to 180°C and held isothermal for 3 minutes to remove thermal history. Next, the sample is cooled to -40°C at a cooling rate of 10°C / min and held isothermal at -40°C for 3 minutes. The sample is then heated to 180°C at a heating rate of 10°C / min (this is the "second heat" ramp). The cooling curve and the second heating curve are recorded. The cooling curve is analyzed by setting a baseline end point from the onset of crystallization to -20°C. The heating curve is analyzed by setting a baseline end point from -20°C to the end of melting. The values ​​determined are the extrapolated onset of melting Tm and the extrapolated onset of crystallization Tc. The heat of fusion (in Joules per gram) (H f ), and the percent crystallinity of the polyethylene sample calculated using the following equation: percent crystallinity = ((H f) / 292 J / g) x 100. The glass transition temperature, Tg, is determined from the DSC heating curve where half of the sample has acquired the heat capacity of a liquid, as described in Bernhard Wunderlich, The Basis of Thermal Analysis, in Thermal Characterization of Polymeric Materials 92, 278-279 (Edith A. Turi ed., 2d ed. 1997). Baselines are drawn below and above the glass transition region and extrapolated through the Tg region. The temperature at which the heat capacity of the sample is halfway between these baselines is the Tg.

[0030] Measure the melt flow rate (MFR) in g / 10 min according to ASTM D1238 (230° C. / 2.16 kg).

[0031] Melt index (MI) (I2) in g / 10 min is measured according to ASTM D1238 (190° C. / 2.16 kg).

[0032] Standardized gas chromatography to measure odor reduction. Odor suppression is the ability of a composition to reduce or otherwise neutralize the amount of volatile hetero-carbonyl species in the composition. Using gas chromatography, (i) the amount of volatile hetero-carbonyl species in the headspace gas around a polymer component sample that does not contain an odor suppressant (hereinafter "undiluted polymer component") is compared to (ii) the headspace gas around a second sample having the same polymer component as the undiluted polymer component (this second sample also contains an amount of odor suppressant). Using the following equation (1), the GC detection value for the headspace gas around the first sample (undiluted polymer component) is compared to the GC detection value for the headspace gas of the second sample (polymer component containing odor suppressant).

[0033] Reaction scheme (1) (GC(PO with odor suppressant at t)-GC(undiluted PO at t)) / GC(undiluted PO at t) x 100 = % odor reduction where GC is the detected gas chromatography value for one or more predetermined volatile carbonyl-containing species; PO is the polymer component; t is a predetermined time interval.

[0034] Equation (1) is hereinafter referred to as "standardized gas chromatography."

[0035] Standardized gas chromatography is performed as follows: The percent concentration of odor producing volatile hetero-carbonyl species is measured by gas chromatography / mass spectrometry (GC / MS).

[0036] An Agilent 7890A gas chromatograph (GC) is used with the following columns: DB-1701, 30 m x 0.32 mm ID x 1 μm film thickness, with helium as the carrier gas at a constant flow rate of 2.0 mL / min. The GC oven is programmed to hold at 50°C for 3.5 minutes. The inlet split temperature is 150°C with a split ratio of 10:1. The headspace gas injection volume is 1.0 mL and is injected using a gas-tight syringe. The transfer line is held at 250°C.

[0037] The column outlet was connected in parallel to a mass spectrometer and a flame ionization detector (FID) through an Agilent 2-Way non-Purged Splitter (part number G3181B). The mass spectrometer was operated with scan 14-200 m / z (EI), source temperature 230 °C, quadrupole temperature 150 °C, EM voltage 2447 V, electron energy -70 eV, two samples, and threshold 0.

[0038] The FID is run under the following conditions: 250° C., hydrogen flow of 30 mL / min, air flow of 400 mL / min, and make-up gas of 45 mL helium / min.

[0039] Samples are prepared by adding 2 grams of sample pellet to a separate headspace vial. No additional chemicals were added to the headspace because all volatile hetero-carbonyl species in the headspace evaporate from the PCR sample. Samples are sealed at room temperature for 20 hours (hrs) and shaken for 4 hours.

[0040] To evaluate odor suppression capacity, headspace gas is collected from the vials at predetermined time intervals. "Percent odor reduction" values ​​(or "% odor reduction") are calculated by (a) subtracting the test sample concentration from the control (undiluted polymer components, PCR+polyolefin) concentration for each volatile hetero-carbonyl species (i.e., potential odorant molecules), and then (b) dividing the remainder of (a) by the control concentration using equation (1) above. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0041] The present disclosure provides a composition. In one embodiment, a composition for controlling odor is provided, comprising a polymer component and an odor control agent. The polymer component comprises a post-consumer resin (PCR) and optionally an olefin-based polymer. The composition comprises 0.15 wt% to 15 wt% of the odor control agent based on the total weight of the composition. The odor control agent comprises (i) 0.05 wt% to 2 wt% of a metal oxide having a band gap greater than 5.0 electron volts (eV) based on the total weight of the composition. The odor control agent further comprises (ii) 0.1 wt% to 13 wt% of an acidic copolymer based on the total weight of the composition. The ratio of the metal oxide to the acidic copolymer is 1:20 to 1:1.

[0042] A(i). Post-consumer resins The polymeric component of the composition includes post-consumer resins (PCR). PCR contains a certain amount of volatile hetero-carbonyl species. The term "post-consumer resins" or "PCR" refers to polymeric materials that have previously been used as consumer or industrial packaging. In other words, PCR is waste plastic. PCR is usually polyolefins, and especially polyethylene. PCR usually includes HDPE packaging such as bottles (milk pots, juice containers), LDPE / LLDPE packaging such as films. PCR also includes residues from its original use, such as paper, adhesives, inks, nylon, ethylene vinyl alcohol (EVOH), polyethylene terephthalate (PET), and other odor-causing agents.

[0043] Non-limiting examples of suitable PCR resins include those sold by Envision Plastics (North Carolina, USA) under the trade names EcoPrime™, PRISMA™, Natural HDPE PCR Resins, Mixed Color and Black HDPE PCR Resins, and those sold under the trade names KWR101-150, KWR101-150-M5-BLK, KWR101-150-M10 BLK, KWR102-8812 BLK, KWR102, KWR102LVW, KWR105, KW620, KWR102-M4, KWR-105M2, KWR105M4, KWR621 Examples of PCR primers sold by KW Plastics (North Carolina, USA) under the names FDA, KWR621-20-FDA, KW308A, KW621, KW621-T10, KW621-T20, KW622-20, KW622-35, KW627C, KW1250G, and KWBK10-NB.

[0044] In one embodiment, the polymeric component is comprised of 100% by weight PCR, where the weight percentage is based on the total weight of the polymeric component.

[0045] A(ii). Olefin polymer In addition to PCR, the polymer component may optionally include an olefin-based polymer. In one embodiment, the olefin-based polymer may be a propylene-based polymer or an ethylene-based polymer. The olefin-based polymer may or may not contain an amount of volatile hetero-carbonyl species. Non-limiting examples of propylene-based polymers include propylene copolymers, propylene homopolymers, and combinations thereof. In one embodiment, the propylene-based polymer is a propylene / α-olefin copolymer. Non-limiting examples of suitable α-olefins include C2 and C4-C 20 α-Olefins or C4-C 10 α-olefins, or C4 to C8 α-olefins. Representative α-olefins include ethylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene.

[0046] In one embodiment, the propylene / α-olefin copolymer is a propylene / ethylene copolymer containing greater than 50% by weight, or 51% by weight, or 55% by weight, or 60% to 70% by weight, or 80% by weight, or 90% by weight, or 95% by weight, or 99% by weight of propylene derived units, based on the weight of the propylene / ethylene copolymer. The propylene / ethylene copolymer contains a reciprocal amount of ethylene derived units, or less than 50% by weight, or 49% by weight, or 45% by weight, or 40% to 30% by weight, or 20% by weight, or 10% by weight, or 5% by weight, or 1% by weight, or 0% by weight of ethylene derived units, based on the weight of the propylene / ethylene copolymer.

[0047] In one embodiment, the olefin-based polymer is an ethylene-based polymer. The ethylene-based polymer can be an ethylene homopolymer or an ethylene / α-olefin copolymer.

[0048] In one embodiment, the ethylene-based polymer is an ethylene / α-olefin copolymer. Non-limiting examples of suitable α-olefins include C3-C 20 α-Olefins or C4-C 10 α-olefins, or C4 to C8 α-olefins. Representative α-olefins include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, and 1-octene.

[0049] In one embodiment, the ethylene / α-olefin copolymer is an HDPE which is an ethylene / C4-C8 α-olefin copolymer. The HDPE has one, some, or all of the following characteristics: (i) a density between 0.940 g / cc and 0.960 g / cc; and / or (ii) a Tm between 128°C and 132°C, and / or (iii) A melt index between 0.5 g / 10 min and 2.0 g / 10 min.

[0050] A non-limiting example of a suitable HDPE is DMDA-1250 available from DowDuPont.

[0051] In one embodiment, the polymer component comprises PCR blended with an olefin-based polymer that is not PCR. In other words, the PCR is blended with a "virgin olefin-based polymer." The virgin olefin-based polymer may or may not contain a certain amount of volatile hetero-carbonyl species. The polymer component may contain from 5% by weight, or 20% by weight, or 30% by weight, or 40% by weight, or 50% by weight, or 60% by weight, or 70% by weight, or 80% by weight, or 95% by weight of PCR and the inverse amount of virgin olefin-based polymer, or from 95% by weight, or 80% by weight, or 70% by weight, or 60% by weight, or 50% by weight to 40% by weight, or 30% by weight, or 20% by weight, or 5% by weight of virgin olefin-based polymer.

[0052] B. Odor Inhibitors The composition includes an odor control agent, which is a blend of a metal oxide (Bi) and an acidic copolymer (Bii).

[0053] B(i) Metal oxides The odor control agent comprises a metal oxide. The metal oxide has a band gap of greater than 5.0 electron volts (eV). As used herein, a "band gap" is the energy range in a solid where no electronic states exist. The band gap is the energy required to promote a "valence electron" to a conduction electron, which is free to move within the crystal lattice and function as a charge carrier to conduct electric current. An "electron volt" or "eV" is approximately 1.6×10 -19 It is a unit of energy equal to a joule. Bandgaps for metal oxides are described in detail in Surface and Nanomolecular Catalysis, Ryan Richards (ed), Taylor & Francis 2006, the contents of which are incorporated herein by reference.

[0054] Without being bound to a particular theory, it is believed that a large band gap (i.e., greater than 5.0 eV) translates into bonds with little covalent character in which electrons are shared disproportionately. This can result in metal ions in the lattice with a net positive charge, and oxide ions with a net negative charge. Thus, the magnitude of the charge can be proportional to the band gap. As a result, the electron-deficient metal ions are free to act as Lewis acids and accept electrons from the slight basic moieties present in the volatile hetero-carbonyl odor molecules. Additionally, the crystalline oxide ions may be able to act as Lewis bases that donate electrons to the slight acidic moieties in the volatile hetero-carbonyl odor molecules.

[0055] Table A below provides band gap values ​​for several metal oxides from Surface and Nanomolecular Catalysis, Ryan Richards (ed), Taylor & Francis 2006. [Table 1]

[0056] In one embodiment, the metal oxide is in particulate (powder) form and has a band gap greater than 5.0 eV, and the metal oxide is selected from calcium oxide (CaO), magnesium oxide (MgO), strontium oxide (SrO), aluminum oxide Al2O3, and combinations thereof.

[0057] In one embodiment, the metal oxide is in the form of particles (powder) and has a band gap of more than 6.0 eV. In a further embodiment, the metal oxide is selected from calcium oxide (CaO), magnesium oxide (MgO), and combinations thereof. In yet a further embodiment, the metal oxide is calcium oxide (CaO).

[0058] In one embodiment, the metal oxide is calcium oxide (6.9 eV) in the form of particles (powder), calcium oxide powder having a D50 particle size of 100 nm to 125 nm, or 150 nm to 250 nm, or 500 nm, or 1000 nm, or 3000 nm. In further embodiments, the calcium oxide powder has a D50 of 100 nm to 3000 nm, or 125 nm to 1000 nm, or 150 nm to 500 nm, or 175 nm to 250 nm, or 125 to 160 nm, or 150 to 160 nm.

[0059] In one embodiment, the metal oxide is hygroscopic and contains moisture bound to its surface, hi a further embodiment, the metal oxide is CaO·H2O.

[0060] B(ii) Acidic Copolymer The odor control agent includes an acidic copolymer with a metal oxide. As used herein, the term "acidic copolymer" (or "AC") is a copolymer containing (i) ethylene monomer and (ii) a carboxylic acid comonomer or its ester derivative (hereinafter referred to as "acidic comonomer"). An acidic copolymer contains an amount of acidic comonomer from 1% by weight, or 5% by weight, or 10% by weight, or 15% by weight to 20% by weight, or 25% by weight, or 30% by weight, and an inverse amount of ethylene monomer. An acidic copolymer is understood to contain more than 50% by weight, or more than 60% by weight of ethylene monomer. In further embodiments, the acidic copolymer comprises 1% to 30% by weight of the acidic comonomer (and inverse ethylene), or 5% to 30% by weight of the acidic comonomer (and inverse ethylene), or 10% to 25% by weight of the acidic comonomer (including inverse ethylene), or 15% to 20% by weight of the acidic comonomer (and inverse ethylene), or 5% to 10% by weight of the acidic comonomer (including inverse ethylene).

[0061] In one embodiment, the acidic comonomer is an acrylate-based moiety. Non-limiting examples of suitable acidic copolymers in which the acidic comonomer is an acrylate-based moiety include ethylene ethyl acrylate copolymer (EEA), ethylene butyl acrylate copolymer (EBA), ethylene acrylic acid copolymer (EAA), ethylene / (meth)acrylic acid copolymer (EMA), and combinations thereof.

[0062] In one embodiment, the acidic copolymer is an ethylene / acrylic acid copolymer having 5% to 30% by weight of acrylic acid comonomer. Non-limiting examples of suitable acidic copolymers include Nucrel® polymers available from EI du Pont de Nemours and Company (Wilmington, Delaware).

[0063] In one embodiment, the odor control agent is a preblend of metal oxide powder dispersed in the acidic copolymer. Mechanical blending and / or melt blending can be used to uniformly distribute the metal oxide particles throughout the acidic copolymer. The odor control agent preblend is then added to the polymer component (A).

[0064] C. Composition In one embodiment, the composition comprises (A) 85% to 99.85% by weight of the polymer component, and (B) 15% to 2%, or 11%, or 10%, or 9%, or 7%, or 5% to 2%, or 1%, or 0.6%, or 0.5%, or 0.3%, or 0.2%, 0.15% by weight of an odor control agent, which is mixed or otherwise blended into the polymer component matrix. The odor control agent contains (i) from 0.05% by weight, or from 0.1% by weight, or from 0.15% by weight, or from 0.2% by weight, or from 0.25% by weight, or from 0.3% by weight, or from 0.4% by weight, or from 0.5% by weight, or from 0.7% by weight, or from 0.9% by weight to 1.0% by weight, or from 1.5% by weight, or from 2% by weight of metal oxide particles (having a band gap of greater than 5.0 eV), and (ii) from 0.1% by weight, or from 0.5% by weight, or from 1.0% by weight, or from 3% by weight, or from 5% by weight, or from 7% by weight, or from 9% by weight to 10% by weight, or from 11% by weight, or from 13% by weight of an acidic copolymer. The weight percentages are based on the total weight of the composition. The ratio of metal oxide to acidic copolymer is from 1:20 to 1:15 to 1:10 to 1:8 to 1:6 to 1:4 to 1:2 to 1:1. The composition exhibits at least a 5% reduction in at least one volatile hetero-carbonyl species compared to the polymer component without the odor control agent (ie, the polymer component alone).

[0065] The reduction in volatile hetero-carbonyl species is a quantitative comparison of the amount of a given volatile hetero-carbonyl species present in (i) the polymer component (i.e., polymer component (A) without the odor control agent) and (ii) the amount of a given volatile hetero-carbonyl species in the present composition comprised of (A) the polymer component and (B) the odor control agent. The reduction in volatile hetero-carbonyl species is measured by standardized gas chromatography as previously disclosed herein.

[0066] As used herein, a "volatile hetero-carbonyl species" is a hydrocarbon compound having 1 carbon atom to 16 carbon atoms that (i) contains at least one heteroatom selected from S, O, N, and / or P, (ii) has a molecular weight of 30 Daltons to 250 Daltons, and (iii) has a vapor pressure of greater than 0.01 millimeters of mercury (mm Hg) at standard temperature and pressure, or "STP." In one embodiment, the volatile hetero-carbonyl species has C-O and / or C=O bonds. Non-limiting examples of volatile hetero-carbonyl species include volatile C1-C 16 Aldehydes, Volatile C1-C 16 Ketones, Volatile C1-C 16 Carboxylic acids, volatile C1-C 16 Esters, Volatile C1-C 16 Alcohol, Volatile C1-C 16 ethers, and combinations thereof.

[0067] Volatile C1~C 16 Non-limiting examples of aldehydes include formaldehyde, acetaldehyde, propanal, hexanal, furfural, heptanal, benzaldehyde, octanal, nonanal, decanal, undecanal, and combinations thereof.

[0068] Volatile C3~C 16 Non-limiting examples of ketones include 2-pentanone, 2-hexanone, 2-octanone, 2-nonanone, 2-decanone, 2-acetophenone, 2-undecanone, and combinations thereof.

[0069] Volatile C1~C 16 Non-limiting examples of carboxylic acids include hexanoic acid, butyric acid, heptanoic acid, octanoic acid, benzoic acid, nonanoic acid, decanoic acid, and combinations thereof.

[0070] Volatile C1~C 16 Non-limiting examples of alcohols include methanol, ethanol, propanol, 2-methylbutanol, and combinations thereof.

[0071] Volatile C1~C 16 Non-limiting examples of ethers include tetrahydrofuran (THF) and its alkyl derivatives.

[0072] In one embodiment, the composition comprises (A) 97% to 98.9% by weight of the polymer component. The composition comprises 3% to 1.1% by weight of an odor control agent, which comprises (Bi) a metal oxide in the form of particles of CaO in an amount of 0.01% to 0.05% by weight, or 0.07% to 0.5% by weight, or 0.7% to 0.9% by weight, and (Bii) an acidic copolymer in an amount of 0.1 to 0.2, or 0.5, or 0.7, or 0.9 to 1.0, or 1.3, or 1.5, or 1.7, or 1.9, and the ratio of the metal oxide to the acidic copolymer is 1:10 to 1:8, or 1:6 to 1:4, or 1:2, or 1:1. The weight percentages are based on the total weight of the composition. The composition exhibits at least a 20% reduction in at least one volatile hetero-carbonyl species compared to a polymer component (A) that does not contain the odor control agent, the reduction in the volatile hetero-carbonyl species being measured by standardized gas chromatography.

[0073] In one embodiment, the composition comprises (A) 98.5 wt% to 99.0 wt% of a polymer component. The composition comprises 1.5 wt% to 1.3 wt% to 1.1 wt%, or 1.0 wt% of an odor control agent, which contains (Bi) a metal oxide which is a particle of CaO in an amount of 0.05 wt% to 0.08 wt% to 0.1 wt%, or 0.13 wt%, or 0.15 wt%, and (Bii) an acid copolymer which is an ethylene / acrylic acid copolymer in an amount of 1.0 wt% to 1.1 wt% to 1.2 wt%, or 1.3 wt%, in which the ratio of metal oxide to acid copolymer is 1:15 to 1:12 to 1:10, or 1:8, hereinafter referred to as Composition 1. The weight percentages are based on the total weight of the composition. Composition 1 exhibits a 10% to 35% reduction in at least one volatile hetero-carbonyl species after a 20 hour exposure period compared to an olefin-based polymer (A) that does not contain an odor inhibitor, the reduction in the volatile hetero-carbonyl species being measured by standardized gas chromatography.

[0074] In one embodiment, composition 1 comprises (A) 98.9 wt% polymer component and 1.1 wt% odor control agent. Polymer component (A) is 90 wt% ethylene-based polymer blended with 10 wt% PCR. The odor control agent contains (Bi) a metal oxide, which is a particle of CaO, in an amount of 0.1 wt%, and (Bii) an acid copolymer, which is an ethylene / acrylic acid copolymer, in an amount of 0.1 wt%, with the ratio of metal oxide to acid copolymer being 1:10. Composition 1 exhibits a greater than 20% reduction in aldehydes compared to the amount of aldehydes present in polymer component (A) alone. The percent reduction in aldehydes is measured by standardized gas chromatography.

[0075] D.Applications The composition can be used in any application where the agent that produces odor or taste from polymeric materials, and in particular the presence of olefin-based polymers, is used in consumer applications.Non-limiting examples of suitable applications for the composition include vehicle interiors, fabrics, and food packaging, including caps, closures, wraps, and bottles.

[0076] Surprisingly, the present composition (i.e., composition 1) exhibits the same or better odor control ability without compromising processability and without compromising film properties. Applicant has discovered that metal oxides with band gaps greater than 5.0 eV work synergistically with acidic copolymers to improve odor control with less total metal oxide (and less CaO) compared to polymer matrix systems containing only metal oxides. The ability of acidic copolymers to synergistically improve odor control when combined with metal oxides (and especially CaO) with band gaps greater than 5.0 eV is unexpected.

[0077] The present disclosure provides a process. In one embodiment, the process includes providing a polymer component (A). The polymer component (A) includes (i) PCR, (ii) an optional olefin-based polymer, and (iii) an amount of at least one volatile carbonyl-containing species. The process includes adding 0.15% to 15% by weight of an odor-inhibiting agent (B) to the polymer component (A). The odor-inhibiting agent (B) includes (Bi) 0.05% to 2% by weight of a metal oxide having a band gap greater than 5.0 electron volts (eV), and (Bii) 0.1% to 13% by weight of an acidic copolymer, the ratio of the metal oxide to the acidic copolymer being 1:20 to 1:1 to form an odor-reducing composition. The process includes neutralizing at least some of the volatile hetero-carbonyl species in the polymer component (A) with the odor-inhibiting agent to form an odor-reducing composition. The weight percentages are based on the total weight of the odor-reducing composition.

[0078] In one embodiment, the process includes forming an odor-reducing composition that exhibits at least a 20% reduction in the amount of volatile hetero-carbonyl species compared to the polymer component (A) without the odor inhibitor as measured by standardized gas chromatography.

[0079] In one embodiment, the process includes dispersing metal oxide particles in the acidic copolymer prior to adding the odor inhibitor preblend to the polymer component (A) to form the odor reducing composition.

[0080] By way of example and not limitation, certain embodiments of the present disclosure will now be described in detail in the following examples. EXAMPLES

[0081] The materials used in the examples are provided in Table 1 below. [Table 2]

[0082] 1. Sample Preparation Melt processing: Modified version of ASTM D1238 using a Tinius Olsen MP600 extrusion plastometer set at 190°C with a weight of 10 Kg. The strands were collected, cut into pieces of approximately 1 cm, reintroduced into the plastometer and extruded a second time (to facilitate more mixing). The resulting second strands were cut into pieces of approximately 1 cm and immediately placed into glass vials sealed with PTFE caps.

[0083] 2. Odor suppression – reduction of volatile hetero-carbonyl species Samples were prepared by adding 2 grams of sample pellets to separate headspace vials. 0.5 mL, 1700 ppmv of propanal sample was added separately to each headspace vial. Samples were sealed at room temperature for 20 hours and shaken for 4 hours. Headspace gas was collected for testing as described above.

[0084] A comparative sample (CS1) was prepared which was a control sample containing polymer components of 90% by weight DMDA1250 (HDPE) and 10% by weight PCR, with no odor control agent.

[0085] IE1 is an inventive example of this composition consisting of 88.9% by weight DMDA1250 (HDPE) and 10% by weight PCR, and 1.1% by weight odor control agent.

[0086] Table 2. Reduction of classes of chemical concentrations in the headspace measured by GC composition (all results normalized to the control sample, CS1). [Table 3]

[0087] The standardized gas chromatography is determined using equation (1) as follows: (GC (20時間でのアルデヒド、CS1) -GC (20時間でのアルデヒド、IE1) ) / GC (20時間でのアルデヒド、CS1) ×100, In the formula, GC (20時間でのアルデヒド、CS1) where t is the area under the curve associated with the aldehyde and t is the time point of 20 h of exposure to volatilized gas from a dose of post-consumer resin equivalent to that used for CS1. The standardized gas chromatography equation (1) is used for ketones, alcohols, THF, and THF derivatives in the same way as for the aldehydes described in this paragraph.

[0088] The odor suppression capacity for CaO is known to be linear, whereby the more CaO added to the polyolefin, the greater the odor suppression. However, high loadings of CaO (greater than 5 wt%) are not preferred, since metal oxides, and especially CaO, can interfere with the melt processing of polyolefins.

[0089] In Table 2, IE1 (odor inhibitor at 1.1 wt%, 0.1 wt% CaO, and 1.0 wt% CaO:AC ratio of 1:10) shows that at lower loadings (less than 0.2 wt% CaO, specifically 0.1 wt% CaO for IE1), the odor inhibitor combined with the 1:10 CaO:AC ratio exhibits a significant amount of odor inhibition (greater than 20% reduction) after 20 hours.

[0090] The present disclosure is not limited to the embodiments and examples contained herein, but is expressly intended to include portions of the embodiments and modifications of these embodiments, including combinations of elements of different embodiments, as falling within the scope of the following claims. The invention as originally claimed in the present application is set forth below. [1] A composition comprising: (i) a post-consumer resin (PCR) and (ii) optionally a polymer component comprising an olefin-based polymer; 0.15% to 15% by weight of an odor control agent, based on the total weight of the composition, (i) 0.05% to 2% by weight, based on the total weight of the composition, of a metal oxide having a band gap greater than 5.0 electron volts (eV); and (ii) 0.1 wt.% to 13 wt.% of an acidic copolymer, based on the total weight of the composition; an odor control agent having a ratio of metal oxide to acidic copolymer of 1:20 to 1:1; A composition comprising: [2] The composition of [1], wherein the composition exhibits at least a 20% reduction in volatile hetero-carbonyl species compared to the polymer component without the odor inhibitor, as measured by standardized gas chromatography. [3] The composition according to any one of [1] to [2], wherein the polymer component contains 100% by weight of a post-consumer resin based on the total weight of the polymer component. [4] The composition according to any one of [1] to [2], wherein the polymer component comprises 5% by weight to 95% by weight of PCR and 95% by weight to 5% by weight of the olefin-based polymer. [5] The composition according to any one of [1] to [4], wherein the olefin-based polymer is selected from the group consisting of ethylene-based polymers, propylene-based polymers, and combinations thereof. [6] The composition according to any one of [1] to [5], wherein the metal oxide is selected from the group consisting of calcium oxide and magnesium oxide. [7] The composition according to any one of [1] to [6], wherein the acidic polymer is selected from the group consisting of ethylene ethyl acrylate copolymer, ethylene butyl acrylate copolymer, ethylene acrylic acid copolymer, ethylene / (meth)acrylic acid copolymer, and combinations thereof. [8] The composition according to any one of [1] to [7], wherein the odor control agent is a preblend of the metal oxide particles dispersed in the acidic copolymer. [9] The composition according to any one of [1] to [8], wherein the metal oxide is calcium oxide particles.

[10] The composition according to any one of [1] to [9], wherein the acidic copolymer is ethylene acrylic acid.

[11] A process comprising: a polymer component comprising (i) a post-consumer resin and (ii) optionally an olefin-based polymer, said polymer component having an amount of at least one volatile hetero-carbonyl species; 0.15% to 15% by weight of an odor control agent, (i) 0.05% to 2% by weight, based on the total weight of the composition, of a metal oxide having a band gap greater than 5.0 electron volts (eV); and (ii) adding to the polymer component an odor control agent comprising 0.1% to 13% by weight of an acidic copolymer based on the total weight of the composition, the ratio of metal oxide to acidic copolymer being 1:20 to 1:1; and neutralizing at least some of the volatile hetero-carbonyl species with said odor control agent to form an odor reducing composition.

[12] The process of

[11] , comprising forming an odor-reducing composition that exhibits at least a 20% reduction in the amount of volatile hetero-carbonyl species compared to the polymer component without the odor inhibitor, as measured by standardized gas chromatography.

[13] prior to said adding, dispersing particles of said metal oxide in said acidic copolymer to form an odor control agent preblend; adding said odor control agent preblend to said polymer component; and forming the odor reducing composition.

Claims

1. 1. A composition comprising: (i) a polymer component consisting of a post-consumer resin (PCR); and (ii) an olefin-based polymer that is an ethylene / C4-C8 α-olefin copolymer; 0.15% to 15% by weight of an odor control agent, based on the total weight of the composition, (i) 0.05 wt % to 2 wt %, based on the total weight of the composition, of a metal oxide having a band gap greater than 5.0 electron volts (eV); and (ii) 0.1 wt. % to 13 wt. % of an acidic copolymer, based on the total weight of the composition; an odor control agent having a ratio of metal oxide to acidic copolymer of 1:20 to 1:1; Including, The metal oxide is calcium oxide. composition.

2. 10. The composition of claim 1, wherein the composition exhibits at least a 20% reduction in volatile hetero-carbonyl species as compared to the polymer component without the odor control agent as measured by standardized gas chromatography.

3. The composition of any one of claims 1 to 2, wherein the polymer component comprises 100% by weight of post-consumer resin, based on the total weight of the polymer component.

4. The composition of any one of claims 1 to 2, wherein the polymer component comprises 5% to 95% by weight of PCR and 95% to 5% by weight of the olefin-based polymer.

5. The composition of any one of claims 1 to 4, wherein the olefin-based polymer is selected from the group consisting of ethylene-based polymers, propylene-based polymers, and combinations thereof.

6. 6. The composition of any one of claims 1 to 5, wherein the acidic copolymer is selected from the group consisting of ethylene ethyl acrylate copolymer, ethylene butyl acrylate copolymer, ethylene acrylic acid copolymer, ethylene / (meth)acrylic acid copolymer, and combinations thereof.

7. The composition of any one of claims 1 to 6, wherein the odor control agent is a preblend of the metal oxide particles dispersed in the acidic copolymer.

8. The composition according to any one of claims 1 to 7, wherein the metal oxide is particles of calcium oxide.

9. The composition of any one of claims 1 to 8, wherein the acidic copolymer is ethylene acrylic acid.

10. A process comprising: a polymer component consisting of (i) a post-consumer resin and (ii) an olefin-based polymer that is an ethylene / C4-C8 α-olefin copolymer, said polymer component having an amount of at least one volatile hetero-carbonyl species; 0.15% to 15% by weight of an odor control agent, (i) 0.05% to 2% by weight, based on the total weight of the odor reducing composition, of a metal oxide having a band gap greater than 5.0 electron volts (eV); and (ii) adding to the polymer component an odor control agent comprising 0.1% to 13% by weight of an acidic copolymer based on the total weight of the odor reducing composition, the ratio of metal oxide to acidic copolymer being 1:20 to 1:1; and neutralizing at least some of the volatile hetero-carbonyl species with the odor control agent to form an odor reducing composition; The metal oxide is calcium oxide. process.

11. 11. The process of claim 10, comprising forming an odor-reducing composition that exhibits at least a 20% reduction in the amount of volatile hetero-carbonyl species compared to the polymer component without the odor-inhibiting agent as measured by standardized gas chromatography.

12. prior to said adding, dispersing said metal oxide particles in said acidic copolymer to form an odor control agent preblend; adding said odor control agent preblend to said polymer component; and forming the odor reducing composition.

Citation Information

Patent Citations

  • Polypropylene composite material and preparation method and application thereof

    CN103374180A

  • Method for inhibiting hydrochloric acid generated during recycling of waste plastic

    JP2006070237A

  • Method for preparing filled polyolefin resins and the resin made therefrom

    US4420580A

  • Method for improving the surface appearance and processing of plastics recovered from durable goods

    WO2014070908A1

  • "thermoplastic polymer formulation containing recycled polyolefins and method of preparing"