Method for producing negative electrode mixture slurry for non-aqueous electrolyte secondary battery
The method enhances the dispersibility and cycle characteristics of negative electrode mixture slurries by precise kneading and solid content control, addressing electrode expansion issues in batteries using carbon-based and Si-based active materials.
Patent Information
- Application Number
- JP2022086579
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-05-27
- Publication Date
- 2024-10-31
- Estimated Expiration
- 2042-05-27
AI Technical Summary
Existing methods using carbon-based and Si-based active materials with polyacrylic acid and carboxymethyl cellulose as binders fail to sufficiently suppress electrode expansion and deterioration in cycle characteristics during battery charging and discharging.
A method for producing a negative electrode mixture slurry involving specific kneading steps and solid content percentages, along with the use of carboxymethyl cellulose and polyacrylic acid, to enhance dispersibility and suppress electrode expansion, ensuring excellent cycle characteristics.
The method results in a negative electrode mixture slurry with improved dispersibility and cycle characteristics, reducing electrode expansion and maintaining battery capacity and reducing pack costs.
Smart Images

Figure 0007576590000002 
Figure 0007576590000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a negative electrode mixture slurry for a non-aqueous electrolyte secondary battery. [Background technology]
[0002] In non-aqueous electrolyte secondary batteries (hereinafter also referred to as "batteries"), a carbon-based active material and a Si-based active material may be used in combination as the negative electrode active material contained in the negative electrode in order to improve the battery capacity. It is known that a negative electrode containing a Si-based active material is prone to deterioration in the cycle characteristics of the battery because it expands and contracts significantly during charging and discharging of the battery. For example, Patent Document 1 discloses that the cycle characteristics of the battery are improved by suppressing the expansion and contraction of the Si-based active material using polyacrylic acid as a binder, and that the storage stability of a slurry composition for forming a negative electrode is improved by also using carboxymethyl cellulose as a binder. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2015 / 098050 Summary of the Invention [Problem to be solved by the invention]
[0004] However, even when a carbon-based active material and a Si-based active material are used as the negative electrode active material and polyacrylic acid and carboxymethyl cellulose are used as the binder, it was sometimes impossible to sufficiently suppress the deterioration of cycle characteristics and the expansion of the electrode due to the charging and discharging of the battery.
[0005] The present disclosure has an object to provide a method for producing a negative electrode mixture slurry that has excellent dispersibility of a negative electrode active material containing a carbon-based active material and a Si-based active material, and that can suppress electrode expansion due to charge and discharge and provide a nonaqueous electrolyte secondary battery having excellent cycle characteristics. [Means for solving the problem]
[0006] The present disclosure provides the following method for producing a negative electrode mixture slurry for a nonaqueous electrolyte secondary battery. [1] A method for producing a negative electrode mixture slurry for a non-aqueous electrolyte secondary battery, comprising: A first step of obtaining a first kneaded body, and a second step of obtaining the negative electrode mixture slurry by using the first kneaded body, The first step includes a step of kneading a negative electrode active material including a carbon-based active material and a Si-based active material, carboxymethyl cellulose, polyacrylic acid, and water, The second step includes a step (x1) of kneading the first kneaded body, carboxymethyl cellulose, and water, When a solid content ratio calculated based on the total weight of the negative electrode active material, the carboxymethyl cellulose, and the polyacrylic acid contained in the first kneaded body and the weight of water contained in the first kneaded body when a torque equivalent to 70% torque oil absorption of the negative electrode active material is generated in the first kneaded body is a [%], The solid content of the first kneaded body is (a-3)% or more and a% or less, The method for producing a negative electrode mixture slurry, wherein the negative electrode mixture slurry has a solid content of (a-15)% or more and (a-10)% or less. [2] The method for producing a negative electrode mixture slurry according to [1], wherein the carbon-based active material contains graphite. [3] The method for producing a negative electrode mixture slurry according to [1] or [2], wherein the second step further includes a step (x2) of adding a binder other than carboxymethyl cellulose to the second kneaded body obtained in the step (x1), and kneading the resulting mixture. [4] The step (x1) mixing carboxymethyl cellulose and water to obtain a mixture; The method for producing a negative electrode mixture slurry according to any one of [1] to [3], further comprising: kneading the first kneaded body and the mixture. [5] The method for producing a negative electrode mixture slurry according to any one of [1] to [4], wherein the kneading time in the first step is 60 minutes or longer. [6] The method for producing a negative electrode mixture slurry according to any one of [1] to [5], wherein the kneading time in the second step is 10 minutes or longer. [7] The method for producing a negative electrode mixture slurry according to any one of [1] to [6], wherein a viscosity of a 1 wt % aqueous solution of carboxymethyl cellulose used in the first step is smaller than a viscosity of a 1 wt % aqueous solution of carboxymethyl cellulose mixed with the first kneaded body in the second step. Effect of the Invention
[0007] According to the present disclosure, it is possible to provide a method for producing a negative electrode mixture slurry that has excellent dispersibility of a negative electrode active material containing a carbon-based active material and a Si-based active material, and that can suppress electrode expansion due to charge and discharge and obtain a nonaqueous electrolyte secondary battery having excellent cycle characteristics. [Brief description of the drawings]
[0008] [Figure 1] 2 is a flowchart showing a method for producing a negative electrode mixture slurry according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] (Method for Producing Negative Electrode Mixture Slurry for Non-Aqueous Electrolyte Secondary Battery) 1 is a flow chart showing a method for producing a negative electrode mixture slurry according to an embodiment. The method for producing a negative electrode mixture slurry according to the present embodiment is a method for producing a negative electrode mixture slurry for a non-aqueous electrolyte secondary battery (hereinafter also referred to as the present battery). The negative electrode mixture slurry is used to form a negative electrode active material layer of the negative electrode of the present battery.
[0010] The negative electrode mixture slurry contains a negative electrode active material, a binder, and water, and may further contain fibrous carbon.
[0011] The negative electrode active material includes a carbon-based active material and a Si-based active material. By including the carbon-based active material and the Si-based active material in the negative electrode active material, the capacity of the battery can be increased compared to the case where only the carbon-based active material is used as the negative electrode active material. Examples of the carbon-based active material include carbon (C) such as graphite, hard carbon, soft carbon, and amorphous coated graphite. Examples of the Si-based active material include silicon alone, a composite of Si and C (such as a composite in which silicon nanoparticles are dispersed in porous carbon particles), SiOx, and LixSiyOz.
[0012] The binder is preferably an aqueous binder that dissolves or disperses in water. Examples of the binder include carboxymethyl cellulose (hereinafter also referred to as "CMC"), polyacrylic acid (hereinafter also referred to as "PAA"), styrene butadiene rubber (hereinafter also referred to as "SBR"), polyethylene oxide (PEO), polyacrylonitrile (PAN), acrylonitrile butadiene rubber (NBR), polytetrafluoroethylene (PTFE), and the like. CMC and PAA may be in the form of an acid or a salt. The negative electrode mixture slurry contains at least CMC and PAA as binders, and may further contain SBR.
[0013] An example of fibrous carbon is carbon nanotubes (hereinafter, also referred to as "CNTs"). The CNTs may be single-walled carbon nanotubes (SWCNTs) or multi-walled carbon nanotubes such as double-walled carbon tubes (DWCNTs).
[0014] The method for producing the negative electrode mixture slurry includes a first step of obtaining a first kneaded body, and a second step of obtaining the negative electrode mixture slurry using the first kneaded body. The first step includes a step of kneading a negative electrode active material, CMC, PAA, and water. The second step includes a step (x1) of mixing and kneading the first kneaded body, CMC, and water. The second step may further include a step (x2) of adding a binder other than CMC to the second kneaded body obtained by the step (x1) and kneading the mixture.
[0015] The solid content rate of the first kneaded body obtained in the first step is (a-3)% or more and a% or less, where a solid content rate under the conditions described below is a%. The step of kneading the negative electrode active material, CMC, PAA, and water in the first step is a step of kneading in a high viscosity state. The solid content rate of the first kneaded body may be (a-2)% or more and a% or less, (a-1)% or more and a% or less, or (a-1)% or more and less than a%. The solid content rate of the first kneaded body is calculated as the weight ratio [%] of the solid content (components other than water) to the weight (total weight) of the first kneaded body.
[0016] The solid content rate of the negative electrode mixture slurry obtained in the second step is (a-15)% or more and (a-10)% or less, where a [%] is the solid content rate under the conditions described below. The second step is performed to adjust the solid content concentration of the negative electrode mixture slurry. The solid content rate of the negative electrode mixture slurry may be (a-14)% or more and (a-10)% or less, (a-14)% or more and (a-11)% or less, or (a-13)% or more and (a-11)% or less. The solid content rate of the negative electrode mixture slurry is calculated as the weight ratio [%] of the solid content (components other than water) to the weight (total weight) of the negative electrode mixture slurry. The solid content rate a [%] is, for example, 60% or more and 75% or less.
[0017] The solid content a [%] is calculated based on the total weight M1 of the negative electrode active material, CMC, and PAA contained in the first kneaded body and the weight M2 of the water contained in the first kneaded body when a torque equivalent to 70% torque oil absorption of the negative electrode active material is generated in the first kneaded body (see the following formula). a[%]={M1 / (M1+M2)}×100
[0018] The 70% torque oil absorption of the negative electrode active material is the 70% torque oil absorption of the negative electrode active material (carbon-based active material and Si-based active material) contained in the first kneaded body. The 70% torque oil absorption of the negative electrode active material is the oil absorption of the negative electrode active material when 70% torque is generated, based on the maximum torque (100% torque) generated when linseed oil is titrated at a constant speed to the negative electrode active material contained in the first kneaded body and the change in viscosity characteristics at that time is measured and recorded by a torque detector.
[0019] Since the Si-based active material expands and contracts greatly during charging and discharging of the battery, the conductive path formed between the Si-based active material and the surrounding negative electrode active material (carbon-based active material or Si-based active material) is easily broken. In the first step, the negative electrode active material, CMC, PAA, and water are kneaded so that the solid content of the first kneaded body falls within the above range, thereby allowing the PAA to function well so as to suppress the disconnection of the conductive path of the Si-based active material during charging and discharging of the battery. In addition, by performing the first step, the expansion of the cell due to repeated charging and discharging of the battery can be suppressed, thereby realizing a low reaction force of the cell and reducing the pack cost of the battery.
[0020] Compared with carbon-based active materials, Si-based active materials tend to generate a large amount of SEI (Solid Electrolyte Interphase) on their surfaces during charging and discharging of the battery, and thus tend to cause a decrease in battery capacity (battery cycle characteristics) during charging and discharging. In the first step, the negative electrode active material, CMC, PAA, and water are kneaded together so that the solid content of the first kneaded body falls within the above range, thereby allowing the CMC to adhere to the surface of the negative electrode active material, and the electrochemically active surface (hereinafter also referred to as "active surface") of the negative electrode active material to be appropriately reduced. This allows the amount of SEI generated during charging and discharging of the battery to be adjusted to an appropriate range, which is believed to suppress a decrease in the cycle characteristics of the battery.
[0021] On the other hand, if the CMC added in the first step is used to reduce the active surface of the negative electrode active material, the amount of CMC that functions to suppress the precipitation of the negative electrode active material in the negative electrode mixture slurry will be reduced. Therefore, in the second step, CMC and water are added to the first kneaded body and kneaded (step (x1)). As a result, the precipitation of the negative electrode active material can be suppressed in step (x1) of the second step, and a negative electrode mixture slurry with excellent dispersibility of the negative electrode active material can be obtained. In addition, by setting the solid content rate of the negative electrode mixture slurry obtained in the second step within the above range, a negative electrode mixture slurry with a viscosity that is easy to apply to a negative electrode current collector when manufacturing a negative electrode can be obtained.
[0022] As described above, in the method for producing the negative electrode mixture slurry, CMC is added in portions and kneaded in the first and second steps. Therefore, in the first step, CMC is used to adjust the active surface of the negative electrode active material, and in the second step, CMC can be used to adjust the dispersibility of the negative electrode active material in the negative electrode mixture slurry. In contrast, when CMC is added in the first step and not added in the second step, the active surface of the negative electrode active material can be adjusted, so it is easy to suppress the deterioration of the cycle characteristics of the battery, but it is difficult to suppress the precipitation of the negative electrode active material in the negative electrode mixture slurry. When CMC is not added in the first step and is added in the second step, it is easy to suppress the precipitation of the negative electrode active material in the negative electrode mixture slurry, but it is difficult to suppress the deterioration of the cycle characteristics of the battery because the active surface of the negative electrode active material cannot be adjusted.
[0023] In the first step, the negative electrode active material, CMC, PAA, and water may be mixed and kneaded to obtain the first kneaded body. Alternatively, in the first step, the negative electrode active material, CMC, and PAA may be mixed to obtain a mixture (e.g., a mixed powder), and water may be added to the mixture and kneaded to obtain the first kneaded body.
[0024] The kneading time in the first step is preferably 60 minutes or more, may be 90 minutes or more, may be 120 minutes or more, and is preferably 180 minutes or more. The kneading time in the first step is usually 300 minutes or less, may be 240 minutes or less. By the kneading time in the first step being within the above range, the active surface of the negative electrode active material can be appropriately reduced, so that the decrease in the battery capacity accompanying the charging and discharging of the present battery can be further easily suppressed. In addition, by the kneading time in the first step being within the above range, the conductive path of the Si-based active material can be further easily suppressed from being cut off accompanying the charging and discharging of the present battery.
[0025] The second step may not include step (x2) as long as it includes step (x1), but preferably includes steps (x1) and (x2). In step (x1), the first kneaded body, CMC, and water may be mixed and kneaded to obtain the second kneaded body, but it is preferable to mix CMC and water to obtain a mixture (e.g., a CMC aqueous solution), and mix and knead this mixture with the first kneaded body to obtain the second kneaded body. In the second step, the second kneaded body obtained as described above may be used as the negative electrode mixture slurry as it is, but the negative electrode mixture slurry may be obtained by performing step (x2) of adding a binder other than CMC to the second kneaded body obtained in step (x1) and kneading it.
[0026] The binder other than CMC added in step (x2) is preferably a binder other than CMC and PAA, and more preferably SBR.
[0027] The kneading time in the second step is preferably 10 minutes or more, may be 15 minutes or more, or may be 20 minutes or more. The kneading time in the second step is not particularly limited, but from the viewpoint of productivity, it is usually 120 minutes or less, and may be 60 minutes or less. When the second step includes a step (x1) and a step (x2), the kneading time in the second step is the total kneading time of the step (x1) and the step (x2). By keeping the kneading time in the second step within the above range, it becomes easier to obtain a negative electrode mixture slurry having excellent dispersibility of the negative electrode active material.
[0028] The viscosity V1 of the 1 wt% aqueous solution of CMC used in the first step is preferably smaller than the viscosity V2 of the 1 wt% aqueous solution of CMC mixed with the first kneaded body in the second step. The viscosities V1 and V2 are measured at a temperature of 25° C. The viscosity V1 may be, for example, 1000 mPa·s or more and 5000 mPa·s or less, 1500 mPa·s or more and 4000 mPa·s or less, 1500 mPa·s or more and 2000 mPa·s or less, or 2000 mPa·s or more and 3000 mPa·s or less, at a temperature of 25° C. The viscosity V2 may be, for example, 2000 mPa·s or more and 9000 mPa·s or less, 3000 mPa·s or more and 8000 mPa·s or less, 300 mPa·s or more and 4000 mPa·s or less, or 6000 mPa·s or more and 8000 mPa·s or less at a temperature of 25° C. The viscosities V1 and V2 of a 1 wt % aqueous solution of CMC can be measured by the procedure described in the Examples below.
[0029] The fibrous carbon that may be contained in the negative electrode mixture slurry may be added when the first kneaded body is obtained in the first step, or may be added when the negative electrode mixture slurry is obtained in the second step, or may be added in both steps. When the fibrous carbon is added in the second step, it may be added in the step (x1), or in the step (x2), or may be added in both steps.
[0030] The viscosity of the negative electrode mixture slurry at a temperature of 25° C. may be 50 Pa·s or more and 270 Pa·s or less, 100 Pa·s or more and 250 Pa·s or less, or 120 Pa·s or more and 200 Pa·s or less. The viscosity of the negative electrode mixture slurry can be measured by the procedure described in the Examples described later.
[0031] (Nonaqueous electrolyte secondary battery) In the present battery, a negative electrode active material layer of a negative electrode and a positive electrode active material layer of a positive electrode face each other with a separator and an electrolyte interposed therebetween. The negative electrode, the positive electrode, and the separator constitute the electrodes of the present battery. The present battery may include an exterior body that contains the electrodes and the electrolyte.
[0032] The negative electrode usually has a negative electrode current collector and a negative electrode active material layer. The negative electrode current collector is, for example, a metal foil made of a copper material such as copper or a copper alloy. The negative electrode active material layer can be obtained by applying the above-mentioned negative electrode mixture slurry to the negative electrode current collector, drying it, and compressing it.
[0033] The positive electrode usually has a positive electrode current collector and a positive electrode active material layer, and the positive electrode current collector is, for example, a metal foil made of an aluminum material such as aluminum or an aluminum alloy. The positive electrode active material layer can be made of a material known in the field of batteries.
[0034] The separator and electrolyte may be made of materials known in the battery field. EXAMPLES
[0035] The present disclosure will be described more specifically below with reference to examples and comparative examples. [Preparation of CMC] The following CMCs were prepared: · BSH-3; Viscosity of 1% by weight aqueous solution at 25°C: 1500-2000 mPa s Etherification degree: 0.65~0.75 · BSH-6; Viscosity of 1% by weight aqueous solution at 25°C: 3000-4000 mPa s Etherification degree: 0.65~0.75 · BSH-12; Viscosity of 1% by weight aqueous solution at 25°C: 6000-8000 mPa s Etherification degree: 0.65~0.75
[0036] Comparative Example 1 87 parts by weight of graphite as a carbon-based active material, 10 parts by weight of a composite of Si and C as a Si-based active material, 1 part by weight of CMC (BSH-6, powder) as a binder, and 1 part by weight of PAA (powder) as a binder were mixed with 53 parts by weight of water (amount relative to 100 parts by weight of negative electrode active material (carbon-based active material and Si-based active material)) and kneaded for 30 minutes with a planetary mixer to obtain a first kneaded body (first step). Next, 34 parts by weight of water (amount relative to 100 parts by weight of negative electrode active material) was added little by little to the first kneaded body and kneaded for 20 minutes to obtain a second kneaded body (second step). 1 part by weight of SBR as a binder was added to the second kneaded body and kneaded for 5 minutes to obtain a negative electrode mixture slurry (second step). Table 1 shows the solid content a and the solid content of the first kneaded body and the negative electrode mixture slurry.
[0037] Comparative Example 2 Except for changing the kneading time for obtaining the first kneaded body to 180 minutes, a negative electrode mixture slurry was obtained in the same manner as in Comparative Example 1. Table 1 shows the solid content a and the solid content of the first kneaded body and the negative electrode mixture slurry.
[0038] Example 1 A negative electrode mixture slurry was obtained in the same manner as in Comparative Example 2, except that the amount of CMC used to obtain the first kneaded body was changed to 0.5 parts by weight, and the 34 parts by weight of water (amount relative to 100 parts by weight of the negative electrode active material) used to obtain the second kneaded body was changed to 34 parts by weight of a 1.5 wt % aqueous solution of CMC (BSH-6, powder). The solid content a and the solid content of the first kneaded body and the negative electrode mixture slurry are shown in Table 1.
[0039] Example 2 A negative electrode mixture slurry was obtained in the same manner as in Example 1, except that 0.5 parts by weight of CMC used to obtain the first kneaded body was changed to 0.7 parts by weight of CMC (BSH-3, powder), and 34 parts by weight of a 1.5% by weight aqueous solution of CMC used to obtain the second kneaded body was changed to 34 parts by weight of a 0.9% by weight aqueous solution of CMC (BSH-12, powder) (amount relative to 100 parts by weight of the negative electrode active material). The solid content a and the solid content of the first kneaded body and the negative electrode mixture slurry are shown in Table 1.
[0040] Comparative Example 3 87 parts by weight of graphite as a carbon-based active material, 10 parts by weight of a composite of Si and C as a Si-based active material, 1 part by weight of CMC (BSH-6, powder) as a binder, 1 part by weight of PAA (powder) as a binder, and 76 parts by weight of water (amount relative to 100 parts by weight of the negative electrode active material) were kneaded with a planetary mixer for 180 minutes to obtain a first kneaded body (first step). Next, 1 part by weight of SBR as a binder was added to the first kneaded body and kneaded for 10 minutes to obtain a negative electrode mixture slurry (second step). Table 1 shows the solid content a and the solid content of the first kneaded body and the negative electrode mixture slurry.
[0041] [Calculation of solid content] (Calculation of solid content a) Linseed oil was titrated at a constant rate against the negative electrode active material (carbon-based active material and Si-based active material) contained in the first kneaded body. At this time, the maximum torque generated when the change in the viscosity characteristics of the negative electrode active material titrated with linseed oil was measured and recorded using a torque detector (S-500, manufactured by Asahi Research Institute Co., Ltd.) was taken as 100% torque. The oil absorption amount when 70% torque was generated was determined as 70% torque oil absorption based on 100% torque. In addition, when the 70% torque oil absorption of graphite, which is a carbon-based active material, and a composite of Si and C, which is a Si-based active material, was measured using the same procedure as above, the 70% torque oil absorption of graphite was 48 ml / 100 g, and the 70% torque oil absorption of the composite of Si and C was 77 ml / 100 g.
[0042] The weight M2 of water contained in the first kneaded body was determined when the first kneaded body generated a torque equivalent to the 70% torque oil absorption amount determined above. The solid content a was calculated based on the total weight M1 of the negative electrode active material and the binder (CMC and PAA) contained in the first kneaded body and the weight M2 of water determined above.
[0043] [Viscosity measurement] (Viscosity of negative electrode mixture slurry) The viscosity of the negative electrode mixture slurry was measured using the following measuring device under the following conditions at a temperature of 25°C and a shear rate of 0.01 sec -1 The viscosity was measured at 100°C (Pa·s). Measurement device: MCR102 (manufactured by Anton Paar) Conditions: Cone plate, flow curve measurement
[0044] (Viscosity of CMC aqueous solution) The viscosity of the CMC aqueous solution (viscosity of a 1 wt % aqueous solution at a temperature of 25° C.) was measured using a BM type viscometer.
[0045] (Calculation of solid content of first kneaded body) It was calculated as the weight ratio [%] of the solid content (negative electrode active material other than water and binder) to the weight of the first kneaded body (total amount of negative electrode active material, binder, and water).
[0046] (Calculation of solid content of negative electrode mixture slurry) It was calculated as the weight ratio [%] of the solid content (negative electrode active material other than water and binder) to the weight of the negative electrode mixture slurry (total amount of negative electrode active material, binder, and water).
[0047] [Evaluation of capacity retention rate and cell thickness increase rate] (Battery Construction) The negative electrode mixture slurry obtained in the examples and comparative examples was applied to a negative electrode current collector, dried and compressed to form a negative electrode active material, and a negative electrode was obtained, which was used to fabricate a non-aqueous electrolyte secondary battery. The cell specifications were a laminate exterior, a laminated electrode, and a capacity of 700 mAh.
[0048] (Calculation of capacity retention rate) A cycle test was carried out by repeating charge and discharge 50 times using the produced battery. The capacity after 1 cycle and the capacity after 50 cycles were measured, and the capacity retention rate was calculated based on the following formula. The results are shown in Table 1. Capacity retention rate [%] = (Capacity after 50 cycles / Capacity after 1 cycle) x 100
[0049] (Calculation of cell thickness increase rate) A cycle test was performed by repeating charge and discharge 300 times using the prepared battery. The cell thickness after 1 cycle and after 300 cycles was measured, and the increase rate of the cell thickness was calculated based on the following formula. The results are shown in Table 1. Cell thickness increase rate [%] = {(cell thickness after 300 cycles / cell thickness after 1 cycle)-1}×100
[0050] [Table 1]
[0051] In Comparative Example 1, the kneading time in the first step is short, and CMC is not added in the second step, so the capacity retention rate of the battery is smaller than that of Examples 1 and 2, and the deterioration of the cycle characteristics of the battery cannot be sufficiently suppressed. In Comparative Example 2, CMC is not added in the second step, so the viscosity of the negative electrode mixture slurry is smaller than that of Examples 1 and 2, and it is considered that the negative electrode active material in the negative electrode mixture slurry has settled. In Comparative Example 3, the solid content rate of the first kneaded body is small, and the first step is not kneaded, and the step of adding and kneading CMC is not performed in the second step, so the capacity retention rate of the battery is smaller than that of Examples 1 and 2, and the increase rate of the cell thickness is large. Therefore, in the battery of Comparative Example 3, the deterioration of the cycle characteristics of the battery cannot be sufficiently suppressed, the reaction force of the cell is large, and it is considered that it is difficult to realize a reduction in the pack cost of this battery.
[0052] The embodiments and examples disclosed herein should be considered to be illustrative and not restrictive in all respects. The scope of the present disclosure is defined by the claims, and it is intended to include all modifications within the meaning and scope of the claims.
Claims
1. A method for producing a negative electrode mixture slurry for a non-aqueous electrolyte secondary battery, comprising: A first step of obtaining a first kneaded body, and a second step of obtaining the negative electrode mixture slurry by using the first kneaded body, The first step includes a step of kneading a negative electrode active material including a carbon-based active material and a Si-based active material, carboxymethyl cellulose, polyacrylic acid, and water, The second step includes a step (x1) of kneading the first kneaded body, carboxymethyl cellulose, and water, A solid content ratio calculated based on a total weight M1 of the negative electrode active material, the carboxymethyl cellulose, and the polyacrylic acid contained in the first kneaded body and a weight M2 of water contained in the first kneaded body when a torque equivalent to 70% torque oil absorption of the negative electrode active material is generated in the first kneaded body is defined as a [%], and the solid content ratio a is calculated based on the total weight M1 of the negative electrode active material, the carboxymethyl cellulose, and the polyacrylic acid contained in the first kneaded body when a torque equivalent to 70% torque oil absorption of the negative electrode active material is generated in the first kneaded body. a [%] = {M1 / (M1+M2)}×100 When calculated by The solid content of the first kneaded body is (a-3)% or more and a% or less, The method for producing a negative electrode mixture slurry, wherein the negative electrode mixture slurry has a solid content of (a-15)% or more and (a-10)% or less.
2. The method for producing a negative electrode mixture slurry according to claim 1 , wherein the carbon-based active material includes graphite.
3. 3. The method for producing a negative electrode mixture slurry according to claim 1 or 2, wherein the second step further includes a step (x2) of adding a binder other than carboxymethyl cellulose to the second kneaded body obtained in the step (x1) and kneading the resulting mixture.
4. The step (x1) mixing carboxymethyl cellulose and water to obtain a mixture; The method for producing a negative electrode mixture slurry according to claim 1 , further comprising: kneading the first kneaded body and the mixture.
5. 3. The method for producing a negative electrode mixture slurry according to claim 1, wherein a kneading time in the first step is 60 minutes or more.
6. 3. The method for producing a negative electrode mixture slurry according to claim 1, wherein a kneading time in the second step is 10 minutes or more.
7. 3. The method for producing a negative electrode mixture slurry according to claim 1, wherein the viscosity of the 1 wt % aqueous solution of carboxymethyl cellulose used in the first step is smaller than the viscosity of the 1 wt % aqueous solution of carboxymethyl cellulose mixed with the first kneaded body in the second step.
Citation Information
Patent Citations
Method for manufacturing battery
JP2012243470A
Method for manufacturing secondary battery electrode
JP2013093240A
Composite particle for secondary battery electrode and manufacturing method thereof, secondary battery electrode material and secondary battery electrode
JP2013251073A
Nonaqueous electrolyte secondary battery
JP2014235856A
Method for manufacturing negative electrode active material slurry for nonaqueous electrolyte secondary battery
JP2015207471A