Bamboo-based and lignin-based hard carbon composite material, preparation method and application
Through the preparation of bamboo-based and lignin-based hard carbon composite materials, the problem of low energy density of sodium-ion batteries is solved, high energy density and Coulombic efficiency are improved, and it meets the requirements of environmental protection and low energy consumption.
Patent Information
- Application Number
- CN202410916155.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-07-09
AI Technical Summary
The energy density of sodium-ion batteries is low, mainly due to the large ionic radius and large mass-to-charge ratio of sodium ions, which leads to phase instability and slow ion transport during the reaction process, which affects the theoretical mass specific capacity of the material and limits sodium-ion batteries. Sodium storage performance.
Bamboo-based and lignin-based hard carbon composites are used as negative electrode materials, and high-density hard carbon materials are prepared through acidic oxidant pretreatment, pre-oxidation, pre-carbonization, pickling, phosphoric acid soaking and high-temperature segmented carbonization. And the conductivity and structural density of the material are improved through CVD carbon coating technology.
It significantly improves the energy density and first charge specific capacity of sodium-ion batteries, improves Coulombic efficiency, meets high energy density and reversibility requirements, and uses sustainable and environmentally friendly biomass raw materials to reduce energy consumption and emissions.
Smart Images

Figure CN118851151A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hard carbon, and in particular relates to a bamboo-based and lignin-based hard carbon composite material, a preparation method and an application thereof. Background Art
[0003] At present, the development of sodium-ion battery technology is in a stage of rapid evolution and innovation. Thanks to the advantages of sodium-ion batteries such as low cost, long cycle, fast charging, friendly environment, excellent high and low temperature performance and safety performance, sodium-ion batteries are developing towards low cost, high density and long life. Although sodium-ion batteries have many advantages, their energy density is lower than that of lithium-ion batteries, about 160Wh / kg, which is only two-thirds of that of lithium iron phosphate batteries. This means that sodium-ion batteries store less energy at the same weight or volume, thus providing sodium-electric vehicles with a shorter range.
[0004] The main reasons for the low energy density of sodium-ion batteries are: sodium ions have a larger ionic radius, which affects the stability of the phase during the reaction, and ion transport and diffusion are slower; the mass-to-charge ratio of sodium ions is relatively large, which reduces the theoretical mass specific capacity of the material; sodium has a higher standard electrode potential. In view of the above reasons, the energy density of sodium-ion batteries can be improved by optimizing the battery structure and the energy density of the material. Sodium-ion batteries are mainly composed of four parts: positive electrode, negative electrode, electrolyte and diaphragm. The structure and performance of the positive and negative electrode materials determine the sodium storage performance of the entire battery, and the negative electrode material accounts for about 16% of the total mass of the battery, which has an important influence on the energy density of the battery, and the energy density is ultimately reflected in the sodium storage capacity of the battery. Because the greater the compaction density of the negative electrode material, the greater the mass of active material that can be placed per unit volume, and the higher the capacity and energy density of the battery.
[0005] Therefore, it is particularly important to improve the capacity of hard carbon anode materials by designing a low-cost, high-density anode material. Summary of the invention
[0006] The first object of the present invention is to provide a method for preparing bamboo-based coated hard carbon, the second object of the present invention is to provide a method for preparing lignin-based coated hard carbon, the third object of the present invention is to provide a method for preparing a bamboo-based and lignin-based hard carbon composite material, the fourth object of the present invention is to provide a negative electrode plate, and the fifth object of the present invention is to provide a battery. The present invention prepares two types of hard carbons, bamboo-based coated hard carbon and lignin-based coated hard carbon, and then mixes the two hard carbons and then uses carbon coating to prepare a hard carbon composite material, which can improve the energy density of sodium ion batteries when applied to sodium ion batteries.
[0007] In order to achieve the above-mentioned object and other related objects, the present invention provides the following technical solutions:
[0008] In a first aspect, the present invention provides a method for preparing bamboo-based coated hard carbon, comprising the following steps:
[0009] Pre-treating the raw material to obtain a pre-treated material; the raw material comprises a bamboo-based biomass raw material;
[0010] The pretreated material is pretreated with an acidic oxidant to obtain an acidic oxidant pretreated material;
[0011] pre-oxidizing the acidic oxidant pretreated material to obtain a pre-oxidized material;
[0012] Pre-carbonizing the pre-oxidized material under a protective atmosphere to obtain a pre-carbonized material;
[0013] crushing the pre-carbonized material to obtain a crushed material;
[0014] The crushed material is firstly acid-washed and then water-washed to obtain a purified material;
[0015] The purified material is soaked in acid, filtered and dried to obtain a soaked material; the acid for the acid soaking includes phosphoric acid;
[0016] The soaked material is mixed evenly with the modifier, and then high-temperature coating and carbonization are carried out under a protective atmosphere to obtain bamboo-based coated hard carbon.
[0017] In a second aspect, the present invention provides a method for preparing a lignin-based coated hard carbon, comprising the following steps:
[0018] Pretreating the raw material to obtain a pretreated material; the raw material comprises a lignin-based biomass raw material;
[0019] The pretreated material is pretreated with an acidic oxidant to obtain an acidic oxidant pretreated material;
[0020] pre-oxidizing the acidic oxidant pretreated material to obtain a pre-oxidized material;
[0021] Pre-carbonizing the pre-oxidized material under a protective atmosphere to obtain a pre-carbonized material;
[0022] The pre-carbonized material is crushed to obtain a crushed material;
[0023] The crushed material is firstly acid-washed and then water-washed to obtain a purified material;
[0024] The purified material is soaked in acid, filtered and dried to obtain a soaked material; the acid for the acid soaking includes phosphoric acid;
[0025] The soaked material is mixed evenly with the modifier, and then subjected to high-temperature coating and carbonization under a protective atmosphere to obtain lignin-based coated hard carbon.
[0026] In a third aspect, the present invention provides a method for preparing a bamboo-based and lignin-based hard carbon composite material, comprising the following steps: preparing a bamboo-based coated hard carbon and a lignin-based coated hard carbon, respectively, mixing the bamboo-based coated hard carbon and the lignin-based coated hard carbon, and then carbon coating to obtain a bamboo-based and lignin-based hard carbon composite material;
[0027] The bamboo-based coated hard carbon is prepared by the aforementioned method for preparing bamboo-based coated hard carbon;
[0028] The lignin-based coated hard carbon is prepared by the aforementioned method for preparing lignin-based coated hard carbon.
[0029] In one embodiment of the present invention, the raw material includes at least one of bamboo and wood.
[0030] In one embodiment of the present invention, when preparing bamboo-based coated hard carbon and when preparing lignin-based coated hard carbon, the pretreatment parameters include: washing the raw materials with water, and then putting them into a drying oven for drying, the drying temperature of the drying oven is 60-120°C, and the drying time is 4-24 hours.
[0031] In one embodiment of the present invention, when preparing bamboo-based coated hard carbon and when preparing lignin-based coated hard carbon, the parameters of pretreating the pretreated material with an acidic oxidant include: reacting the pretreated material and the acidic oxidant at 60-100°C for 4-12 hours, the acidic oxidant includes an oxidant and an acid, the oxidant includes at least one of hydrogen peroxide, peracetic acid, and ozone, wherein the concentration of the oxidant is 1-5%, the acid includes at least one of formic acid and acetic acid, the concentration of the acid is 0.5-2%, and the solid-liquid mass ratio of the pretreated material and the acidic oxidant is 1:1.2-5.
[0032] In one embodiment of the present invention, when preparing bamboo-based coated hard carbon and lignin-based coated hard carbon, the acidic oxidant pretreated material is pre-oxidized, and the parameters of the pre-oxidized material include: temperature of 200-350°C, and pre-oxidation time of 3-5h.
[0033] In one embodiment of the present invention, when preparing bamboo-based coated hard carbon and when preparing lignin-based coated hard carbon, the pre-oxidized material is pre-carbonized under a protective atmosphere, and the parameters of the pre-carbonized material include: a heating rate of 2 to 10°C / min, a pre-carbonization temperature of 200 to 800°C, and a holding time of 1 to 3h. The pre-carbonization is carried out in a rotary kiln, and the protective atmosphere includes at least one of nitrogen, argon, and helium.
[0034] In one embodiment of the present invention, when preparing bamboo-based coated hard carbon and when preparing lignin-based coated hard carbon, the pre-carbonized material is crushed, and the parameters of the crushed material include: the equipment used for the crushing includes at least one of a mechanical crusher, a roller mill crusher, and a jet crusher, and the particle size D50 of the crushed material is controlled at 3 to 10 um.
[0035] In one embodiment of the present invention, when preparing bamboo-based coated hard carbon and when preparing lignin-based coated hard carbon, the crushed material is first pickled and then washed with water, and the parameters of the purified material include: the pickling acid includes at least two of hydrochloric acid, nitric acid, hydrofluoric acid, and sulfuric acid; the acid concentration of the pickling is 20-50%, the reaction temperature of the pickling is 60-100°C, the solid-liquid mass ratio of the pickling is 1:0.7-5.5, and the pickling time is 4-24h; the washing process includes: multiple deionized water washing until the filtrate is close to neutral, and then filtered and dried, the drying temperature is 60-120°C, and the drying time is 6-24h.
[0036] In one embodiment of the present invention, when preparing bamboo-based coated hard carbon and when preparing lignin-based coated hard carbon, the purified material is immersed in a phosphoric acid solution, and the parameters of the immersed material include: the concentration of the phosphoric acid is 3-30%, the immersion time is 3-24h, and the solid-liquid mass ratio is 1:1.2-3; stirring is performed while immersing, and after immersion, filtration and drying are performed, the drying temperature is 60-120°C, and the drying time is 4-24h.
[0037] In one embodiment of the present invention, when preparing bamboo-based coated hard carbon and lignin-based coated hard carbon, the soaked material is evenly mixed with a modifier, and then high-temperature coating and carbonization are carried out under a protective atmosphere. The parameters include: the modifier includes at least one of asphalt and resin, and the mass of the modifier accounts for 1 to 10 wt% of the mass of the soaked material; the mixing time is 0.5 to 3 hours.
[0038] High-temperature coating carbonization is high-temperature segmented carbonization: the first stage is low-temperature carbonization, the temperature is 800-1000°C, the heating rate is 4-6°C / min, and the constant temperature time is 1-2h; the second stage is high-temperature carbonization, the temperature is 1200-1400°C, the heating rate is 1-2°C / min, and the constant temperature time is 2-4h; the third stage is cooling, cooling to 800-1100°C, the cooling rate is 3-5°C / min, and the protective atmosphere is continued to cool naturally to 25-30°C.
[0039] The protective atmosphere includes at least one of nitrogen, argon and helium.
[0040] In one embodiment of the present invention, when the bamboo-based coated hard carbon and the lignin-based coated hard carbon are mixed and then carbon-coated to obtain the bamboo-based and lignin-based hard carbon composite material, the bamboo-based coated hard carbon and the lignin-based coated hard carbon are mixed and then added to the CVD carbon coating equipment, and then the carbon source and the protective gas are introduced, the temperature is increased, the temperature is kept, and the temperature is cooled to obtain the bamboo-based and lignin-based hard carbon composite material;
[0041] Among them, the mass ratio of the bamboo-based coated hard carbon and the lignin-based coated hard carbon is 1:9-9:1, the mixing time is 0.5-2h, the carbon source includes at least one of acetylene, methane, propane, ethylene, propylene, and benzene, the protective gas includes at least one of argon and nitrogen, the volume fraction of the carbon source and the protective gas is 4%-10%:96%-90%, the heating rate is 5-10℃ / min, the heating temperature is 650-1000℃, and the insulation time is 0.5-4h; the CVD carbon coating equipment includes at least one of a CVD rotary furnace, an intermittent vapor deposition CVD furnace, and a continuous vapor deposition CVD furnace.
[0042] Furthermore, the powder compaction density of bamboo-based and lignin-based hard carbon composite materials is 0.8900-1.2000 g / cm 3 .
[0043] In a fourth aspect, the present invention provides a negative electrode plate, wherein the negative electrode plate uses a bamboo-based and lignin-based hard carbon composite material as an active substance of a battery negative electrode material, and the bamboo-based and lignin-based hard carbon composite material is prepared by the aforementioned preparation method of the bamboo-based and lignin-based hard carbon composite material.
[0044] In a fifth aspect, a battery is provided, which is a sodium ion battery, comprising a negative electrode, a positive electrode, a separator, and an electrolyte. The negative electrode comprises the aforementioned negative electrode plate. A charge and discharge test is performed at a current density of 0.1C. The first charge specific capacity of the sodium ion battery is greater than 330mAh / g, and the first coulombic efficiency is greater than 90%.
[0045] The above-mentioned negative electrode plate and battery are applications of bamboo-based and lignin-based hard carbon composite materials.
[0046] The beneficial effects of the present invention are:
[0047] 1. Environmental protection of raw materials: The bamboo-based biomass raw materials and lignin-based biomass raw materials used in the present invention are a kind of green material with abundant resources, short growth cycle and renewable nature. They have excellent characteristics such as wide distribution, fast growth, early maturity and high strength. They are the biomass resources with the largest reserves on the earth. Through photosynthesis, they can produce up to tens of billions of tons of bamboo-based and lignin-based biomass raw materials every year, which can ensure a stable supply of raw materials. In addition, as a sustainable and environmentally friendly material, the preparation process of bamboo-based and lignin-based biomass raw materials has the characteristics of low energy consumption and low emissions, which meets the current green development needs. Therefore, the use of bamboo-based and lignin-based biomass raw materials to prepare hard carbon negative electrodes can not only improve energy utilization, but also help reduce dependence on fossil fuels and promote the realization of energy transformation.
[0048] 2. The process of the present invention is reasonable, including pretreatment, acidic oxidant pretreatment, preoxidation, precarbonization, crushing, water washing after acid washing, filtering and drying after acid soaking, modification by modifier, high temperature coating carbonization (high temperature segmented carbonization), and CVD carbon coating, which are as follows:
[0049] (1) Due to the complex and dense structure of the lignocellulose cell wall of lignin-based biomass raw materials, it is difficult to dissolve and utilize. Therefore, the lignocellulose of the present invention adopts a pretreatment method combining an oxidant and an acid. The green strong oxidant can oxidize and degrade the lignocellulose into aldehydes, phenols, organic acids, and small molecular compounds, thereby realizing the separation of carbohydrates, cellulose, hemicellulose, and lignin in the lignocellulose; the acid can promote the decomposition of lignocellulose under mild reaction conditions without high temperature or high pressure, which reduces energy consumption, reduces the risk of side reactions, and improves the availability of lignocellulose. The synergistic effect of the oxidant and the acid destroys the connection between cellulose, lignin, and hemicellulose, and realizes the separation of the components of lignocellulose, which is beneficial to reduce crystallinity and acid washing and impurity removal, improve porosity, hydrolysis efficiency, and raw material utilization, thereby increasing the active sites of the hard carbon composite material, increasing the interlayer spacing, and greatly improving the reversible specific capacity of the battery, and ultimately improving the energy density and specific capacity. The present invention does not adopt a single pretreatment technology, but combines the combined pretreatment of oxidants and acids to overcome the shortcomings of a single method, enhance the pretreatment technology, and effectively improve the resource efficiency of biomass raw materials.
[0050] (2) The biomass raw materials used in the present invention are bamboo-based and lignin-based, and the main component is cellulose. Lignocellulose is mainly composed of cellulose, hemicellulose and lignin, of which cellulose accounts for about 30-50%, lignin and hemicellulose account for 10-20% and 15-35% respectively. The cellulose in cellulose forms microfibers, which constitute the three-dimensional network skeleton of the fiber cell wall, while hemicellulose and lignin are filled between the fibers and microfibers in the form of covalent bonds. Its unique structure and pore channels as well as rich aromatic carbon rings make it a great advantage as a precursor of hard carbon materials for sodium ion batteries. However, the cellulose hard carbon materials obtained by direct carbonization cannot show good electrochemical performance due to their relatively low conductivity and cross-linking degree and fewer sodium ion storage sites. Therefore, the present invention adds a low-temperature pre-oxidation process before pre-carbonization, introduces oxygen-containing, hydroxyl and carbonyl functional groups, and enhances the cross-linking degree between cellulose molecules in the form of ester groups, thereby producing a large number of disordered structures, expanding the carbon layer spacing, and promoting Na + The small molecule gas released during heating will induce the formation of nanopores inside the amorphous carbon, significantly improving the electrochemical properties of the hard carbon composite material.
[0051] (3) The present invention uses phosphoric acid soaking to further dissolve and decrystallize cellulose, hemicellulose and lignin, and also introduces P element doping modification to enhance the reaction activity. + The number of storage sites increases, and the conductivity and wettability are improved, thereby increasing the specific capacity of the hard carbon negative electrode material.
[0052] (4) The present invention does not adopt the method of mixing first and then coating and carbonizing with a modifier, but adopts the method of coating and carbonizing the two materials separately with a modifier first, and then mixing the coated and carbonized materials. This is because the hard carbon precursors are different, and their internal microstructures, pore sizes, pore structures, surface areas, and surface functional groups are different, so that the optimal proportions of each coating are different. The composite material obtained by coating and carbonizing the precursors separately first and then mixing the coated and carbonized precursors can give full play to their respective advantages through the synergistic effect, which can not only make the coating of the hard carbon precursor more uniform and denser, but also maintain the high capacity of bamboo-based biomass and the high compaction of lignin-based biomass.
[0053] (5) The reason for the high-temperature segmented carbonization of the present invention: During the first stage of low-temperature carbonization, pyrolysis occurs, and a large number of organic molecules are quickly released, which is conducive to the formation of a rich pore structure; during the second stage of high-temperature carbonization, the degree of graphitization can be improved and a larger interlayer spacing can be retained, which is conducive to the embedding and extraction of sodium ions in the material, thereby improving the initial coulombic efficiency and reversible capacity. However, the heating rate in the high-temperature stage should not be too fast, otherwise it will easily cause insufficient volatilization of small molecules and increase the specific surface area; during the third stage of cooling, the temperature should be kept slowly lowered, otherwise it will cause internal cracks and reduce performance.
[0054] (6) Compared with solid phase coating, the present invention adopts CVD method for carbon coating. High temperature pyrolysis causes the carbon source gas to be deposited on the surface and in the pores of the bamboo-based and lignin-based hard carbon mixed materials, so that the components of the deposited carbon material are uniform and the structure is dense. The coating layer can not only increase the conductivity of the composite material, but also reduce the decomposition of the electrolyte on the electrode surface, and at the same time has good cycle characteristics.
[0055] 3. The powder compaction density of the bamboo-based and lignin-based hard carbon composite material of the present invention is 0.8900-1.2000 g / cm 3 When applied to negative electrode plates and sodium-ion batteries, it can improve the energy density of sodium-ion batteries. In charge and discharge tests at a current density of 0.1C, the first charge specific capacity of the sodium-ion battery is greater than 330mAh / g, and the first coulomb efficiency is greater than 90%. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0057] Figure 1 is a comparison chart of XRD of the hard carbon composite material of Example 1 of the present invention and Comparative Example 1;
[0058] Figure 2 It is a comparison chart of the charge and discharge curves of the hard carbon composite material of Example 1 of the present invention and Comparative Example 7 under 0.1C conditions. DETAILED DESCRIPTION
[0059] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0060] Unless otherwise specified, the equipment and materials used in the examples can be easily obtained from commercial companies.
[0061] The model of CVD rotary furnace is: KY-RJ(Q) series, Keyuan.
[0062] The model of intermittent vapor deposition CVD furnace is: KY-R-JQC series, Keyuan.
[0063] The model of continuous vapor deposition CVD furnace is: KY-R-LQC series, Keyuan.
[0064] Phenolic resin, cas9003-35-4, Aladdin reagent;
[0065] CMC (sodium carboxymethyl cellulose), cas9004-32-4, C104985, Aladdin reagent;
[0066] Conductive carbon black (SP) and SBR (styrene-butadiene rubber) are both general reagents suitable for batteries.
[0067] Example 1
[0068] A method for preparing a bamboo-based and lignin-based hard carbon composite material, the preparation steps are as follows:
[0069] Note: Because the preparation methods of the bamboo-based coated hard carbon and the lignin-based coated hard carbon are the same in this embodiment (except for the different raw materials), they are uniformly described in the following S1 to S7, and S8 and S9 are further processed using the bamboo-based coated hard carbon and the lignin-based coated hard carbon obtained respectively, specifically:
[0070] S1. Rinse the bamboo or wood with water first, then put it into a drying oven and dry it at 80°C for 24 hours to obtain a pretreated material;
[0071] S2, adding the pretreated material to a mixed solution of 1% formic acid and 3% H2O2 (hydrogen peroxide), reacting at 80°C for 6 hours, wherein the solid-liquid mass ratio is 1:2, to obtain an acidic oxidant pretreated material;
[0072] S3, placing the acidic oxidant pretreated material in a rotary kiln, first introducing oxygen, then heating to 300°C at a heating rate of 3°C / min, pre-oxidizing for 3 hours to obtain a pre-oxidized material, then introducing nitrogen, and heating to 700°C at a heating rate of 5°C / min in a nitrogen atmosphere, keeping the temperature for 2 hours, and then cooling to room temperature to obtain a pre-carbonized material;
[0073] S4, crushing the pre-carbonized material with a jet mill, and controlling the particle size D50 of the particles after crushing to be 5 μm to obtain a crushed material;
[0074] S5. The crushed material is placed in an acid with a concentration of 30%, the acid is an aqueous solution of HCl (hydrochloric acid) and HF (hydrofluoric acid), and reacted at 80°C for 12 hours, wherein the solid-liquid mass ratio is 1:3. After purification, it is first washed with deionized water for several times until the filtrate is close to neutral, and then filtered and placed in a drying oven, and dried at 80°C for 24 hours to obtain a purified material; it should be noted that hydrochloric acid and hydrofluoric acid can be mixed to obtain a concentration of 30%, and the concentration of hydrochloric acid and hydrofluoric acid added separately is not a key feature or does not affect the test results, so it is not elaborated in detail;
[0075] S6, adding 10% phosphoric acid to the purified material and soaking it at room temperature, stirring it while soaking, and after soaking for 6 hours, first filtering it and then placing it in a drying oven at 80°C for 24 hours, wherein the solid-liquid mass ratio is 1:2, to obtain the soaked material;
[0076] S7, the soaked material obtained was mixed with phenolic resin at room temperature using a VC machine, wherein the mass of the phenolic resin was 5wt% of the total mass of the soaked material, and after mixing for 1 hour, the mixture was put into a push plate furnace for high-temperature segmented carbonization. In a nitrogen atmosphere, the temperature was first increased to 800°C at a heating rate of 5°C / min and kept constant for 1 hour; then the temperature was increased to 1300°C at a heating rate of 2°C / min and kept constant for 3 hours; finally, the temperature was reduced to 800°C at a cooling rate of 4°C / min and then naturally cooled to 30°C to obtain bamboo-based or lignin-based hard carbon;
[0077] S8. Mix the bamboo-based coated hard carbon and the lignin-based coated hard carbon in a mass ratio of 3:7 at room temperature using a VC machine. After mixing for 30 minutes, remove iron and pass through a 325-mesh sieve to obtain a bamboo-based and lignin-based hard carbon mixture.
[0078] S9. Add the bamboo-based and lignin-based hard carbon mixture into a continuous vapor phase vapor deposition CVD furnace, then introduce a mixed gas of acetylene and argon with a volume ratio of 4%:96%, increase the temperature to 800°C at a heating rate of 10°C / min, keep warm at 800°C for 1 hour, and then cool to room temperature to obtain a bamboo-based and lignin-based hard carbon composite material.
[0079] Application: The bamboo-based and lignin-based hard carbon composite materials prepared above are used as active materials of battery negative electrode materials in sodium ion batteries.
[0080] According to the mass ratio of 2.0%:4.0%:92.0%:2.0%, 0.2g of CMC (sodium carboxymethyl cellulose), 0.4g of SP (conductive carbon black), 9.2g of bamboo-based and lignin-based hard carbon composite materials, and 0.5g of SBR (styrene-butadiene rubber, solid content 40%) were weighed, and an appropriate amount of deionized water was added. The mixture was stirred for 8 hours until a uniform slurry was formed. The mixture was evenly coated on the surface of the copper foil using a four-sided preparation device, and dried in a vacuum drying oven at 80°C for 8 hours. The Cu foil with active materials was cut into disc-shaped negative electrode sheets, which were then transferred to a glove box for standby use.
[0081] The assembly of button cells was carried out in a glove box with Ar atmosphere, using the prepared bamboo-based and lignin-based hard carbon composites as the negative electrode, 1.0 mol / L commercial electrolyte, the commercial electrolyte was prepared as follows: NaPF6 was added to a volume ratio of EC:DMC=1:1, Na metal sheet or sodium metal block was used as the counter electrode, CR2032 button cells were assembled, and then charge and discharge tests were carried out at a current density of 0.1C.
[0082] It should be noted that the use of a Na metal sheet or a sodium metal block as a counter electrode does not affect the final experimental results in the present invention.
[0083] Example 2
[0084] In this embodiment, different from Embodiment 1, S2 is as follows:
[0085] S2. Add the pretreated material to a mixed solution of 2% formic acid and 5% H2O2, react at 80°C for 6 hours, wherein the solid-liquid mass ratio is 1:2, to obtain an acidic oxidant pretreated material.
[0086] The remaining steps are the same as those in Example 1.
[0087] Example 3
[0088] In this embodiment, different from Embodiment 1, S2 is as follows:
[0089] S2. Add the pretreated material to a mixed solution of 0.5% formic acid and 1% H2O2, react at 80°C for 6 hours, wherein the solid-liquid mass ratio is 1:2, to obtain an acidic oxidant pretreated material.
[0090] The remaining steps are the same as those in Example 1.
[0091] Example 4
[0092] In this embodiment, different from Embodiment 1, S3 is as follows:
[0093] S3. Place the acidic oxidant pretreated material in a rotary kiln, introduce oxygen first, then increase the temperature to 200°C at a heating rate of 3°C / min, pre-oxidize for 5 hours to obtain a pre-oxidized material, then introduce nitrogen, and in a nitrogen atmosphere, increase the temperature to 700°C at a heating rate of 5°C / min, keep warm for 2 hours, and then cool to room temperature to obtain a pre-carbonized material.
[0094] The remaining steps are the same as those in Example 1.
[0095] Example 5
[0096] In this embodiment, different from Embodiment 1, S4 is as follows:
[0097] S4. The pre-carbonized material is crushed by a jet mill, and the particle size D50 of the particles after crushing is controlled at 7 μm to obtain a crushed material.
[0098] The remaining steps are the same as those in Example 1.
[0099] Example 6
[0100] In this embodiment, different from Embodiment 1, S6 is as follows:
[0101] S6. Add 30% phosphoric acid to the purified material and soak it at room temperature while stirring. After soaking for 6 hours, filter it and then place it in a drying oven at 80°C for 24 hours, wherein the solid-liquid mass ratio is 1:2, to obtain the soaked material.
[0102] The remaining steps are the same as those in Example 1.
[0103] Example 7
[0104] In this embodiment, different from Embodiment 1, S7 is as follows:
[0105] S7. Mix the soaked material and phenolic resin uniformly with a VC machine at room temperature, wherein the mass of the phenolic resin is 3wt% of the total mass of the raw material after the bamboo-based soaking or 5wt% of the total mass of the raw material after the lignin-based soaking. After mixing for 1 hour, put it into a push plate furnace for high-temperature segmented carbonization. Under a nitrogen atmosphere, first increase the temperature to 800°C at a heating rate of 5°C / min and keep the temperature constant for 1 hour; then increase the temperature to 1300°C at a heating rate of 2°C / min and keep the temperature constant for 3 hours; finally, reduce the temperature to 800°C at a cooling rate of 4°C / min and then naturally cool to 30°C to obtain bamboo-based or lignin-based coated hard carbon.
[0106] The remaining steps are the same as those in Example 1.
[0107] Note: To avoid ambiguity, when the mass of phenolic resin is 3wt% of the total mass of the raw material after bamboo-based soaking, bamboo-based coated hard carbon is obtained; when the mass of phenolic resin is 5wt% of the total mass of the raw material after lignin-based soaking, lignin-based coated hard carbon is obtained.
[0108] Example 8
[0109] In this embodiment, different from Embodiment 7, S7 is as follows:
[0110] S7. Mix the soaked material and phenolic resin uniformly with a VC machine at room temperature, wherein the mass of the phenolic resin is 5wt% of the total mass of the raw material after the bamboo-based soaking or 3wt% of the total mass of the raw material after the lignin-based soaking. After mixing for 1 hour, put it into a push plate furnace for high-temperature segmented carbonization. Under a nitrogen atmosphere, first increase the temperature to 800°C at a heating rate of 5°C / min and keep the temperature constant for 1 hour; then increase the temperature to 1300°C at a heating rate of 2°C / min and keep the temperature constant for 3 hours; finally, reduce the temperature to 800°C at a cooling rate of 4°C / min and then naturally cool to 30°C to obtain bamboo-based or lignin-based coated hard carbon.
[0111] The remaining steps are the same as those in Example 1.
[0112] Note: To avoid ambiguity, when the mass of phenolic resin is 5wt% of the total mass of the raw material after bamboo-based soaking, bamboo-based coated hard carbon is obtained; when the mass of phenolic resin is 3wt% of the total mass of the raw material after lignin-based soaking, lignin-based coated hard carbon is obtained.
[0113] Example 9
[0114] In this embodiment, different from Embodiment 1, S8 is as follows:
[0115] S8. Mix the bamboo-based coated hard carbon and the lignin-based coated hard carbon in a mass ratio of 7:3 using a VC machine at room temperature. After mixing for 30 minutes, remove iron and pass through a 325-mesh sieve to obtain a bamboo-based and lignin-based hard carbon mixture.
[0116] The remaining steps are the same as those in Example 1.
[0117] Example 10
[0118] In this embodiment, different from Embodiment 1, S8 is as follows:
[0119] S8. Mix the bamboo-based coated hard carbon and the lignin-based coated hard carbon in a mass ratio of 5:5 at room temperature using a VC machine. After mixing for 30 minutes, remove iron and pass through a 325-mesh sieve to obtain a bamboo-based and lignin-based hard carbon mixture.
[0120] The remaining steps are the same as those in Example 1.
[0121] Embodiment 11
[0122] In this embodiment, different from Embodiment 1, S8 is as follows:
[0123] S8. Mix the bamboo-based coated hard carbon and the lignin-based coated hard carbon in a mass ratio of 4:6 using a VC machine at room temperature. After mixing for 30 minutes, remove iron and pass through a 325-mesh sieve to obtain a bamboo-based and lignin-based hard carbon mixture.
[0124] The remaining steps are the same as those in Example 1.
[0125] Example 12
[0126] In this embodiment, different from Embodiment 1, S8 is as follows:
[0127] S8. Mix the bamboo-based coated hard carbon and the lignin-based coated hard carbon in a mass ratio of 6:4 at room temperature using a VC machine. After mixing for 30 minutes, remove iron and pass through a 325-mesh sieve to obtain a bamboo-based and lignin-based hard carbon mixture.
[0128] The remaining steps are the same as those in Example 1.
[0129] Comparative Example 1
[0130] A method for preparing a bamboo-based and lignin-based hard carbon composite material, compared with Example 1, the difference is that: there is no acidic oxidant pretreatment process in step 2, that is, the pretreated material obtained in step S1 is directly processed in step S3.
[0131] The rest of the steps are consistent with those in Example 1, and the obtained battery material is tested using the same method as in Example 1.
[0132] Comparative Example 2
[0133] A method for preparing a bamboo-based and lignin-based hard carbon composite material, compared with Example 1, the difference is that there is no pre-oxidation process in step 3, and direct pre-carbonization:
[0134] S3. Place the acidic oxidant pretreated material in a rotary kiln, introduce nitrogen, and heat the temperature to 700°C at a heating rate of 5°C / min under a nitrogen atmosphere. Keep the temperature for 2 hours and then cool to room temperature to obtain a pre-carbonized material.
[0135] The rest of the steps are consistent with those in Example 1, and the obtained battery material is tested using the same method as in Example 1.
[0136] Comparative Example 3
[0137] A method for preparing a bamboo-based and lignin-based hard carbon composite material, compared with Example 1, the difference is that: there is no phosphoric acid soaking process in step 6, and the purified material obtained in step S5 is directly processed in step S7.
[0138] The rest of the steps are consistent with those in Example 1, and the obtained battery material is tested using the same method as in Example 1.
[0139] Comparative Example 4
[0140] A method for preparing a bamboo-based and lignin-based hard carbon composite material, compared with Example 1, the difference is that: in step S7, the obtained soaked material and phenolic resin are mixed evenly with a VC machine at room temperature, wherein the mass of the phenolic resin is 5wt% of the total mass of the soaked material; after mixing for 1 hour, the mixture is put into a push plate furnace and heated from room temperature to 1300°C at a heating rate of 2°C / min under a nitrogen atmosphere for 3 hours, and then naturally cooled to room temperature; the rest are consistent with the steps of Example 1, and the obtained battery material is tested by the same method as Example 1.
[0141] Comparative Example 5
[0142] A method for preparing a bamboo-based and lignin-based hard carbon composite material, compared with Example 1, has the following differences:
[0143] Step S1 is to rinse the bamboo with water first, and then put it into a drying oven and dry it at 80°C for 24 hours to obtain a pretreated material; Step S7 is to mix the obtained bamboo-based soaked material with phenolic resin at room temperature using a VC machine, wherein the mass of the phenolic resin is 5wt% of the total mass of the raw material, and the raw material is placed in a push plate furnace after mixing for 1 hour, and in a nitrogen atmosphere, the temperature is increased to 1300°C at a heating rate of 2°C / min for high-temperature coating and carbonization, and the heat preservation time is 3 hours. After cooling to room temperature, a bamboo-based coated hard carbon material is obtained, and there is no step 8. Step S9 is to add the bamboo-based coated hard carbon material to a continuous gas phase vapor deposition CVD furnace, and then introduce a mixed gas of acetylene and argon with a volume ratio of 4%:96%, and the temperature is increased to 800°C at a heating rate of 10°C / min, and after being kept at 800°C for 1 hour, it is cooled to room temperature to obtain a bamboo-based hard carbon composite material. The rest are consistent with the steps of Example 1, and the obtained battery material is tested by the same method as Example 1 (during the test preparation, the bamboo-based hard carbon composite material replaces the bamboo-based and lignin-based hard carbon composite materials).
[0144] It should be noted that, in this embodiment, lignin-based coated hard carbon was not prepared.
[0145] Comparative Example 6
[0146] A method for preparing a bamboo-based and lignin-based hard carbon composite material, compared with Example 1, has the following differences:
[0147] Step S1 is to rinse the wood with water, and then put it into a drying oven and dry it at 80°C for 24 hours to obtain a pretreated material; Step S7 is to mix the obtained lignin-based soaked material with phenolic resin at room temperature using a VC machine, wherein the mass of the phenolic resin is 5wt% of the total mass of the raw material, which is the lignin-based soaked material; after mixing for 1 hour, it is placed in a push plate furnace, and in a nitrogen atmosphere, the temperature is increased to 1300°C at a heating rate of 2°C / min for high-temperature coating and carbonization, and the heat preservation time is 3 hours. After cooling to room temperature, a lignin-based coated hard carbon material is obtained, and there is no step 8. Step S9 is to add the lignin-based coated hard carbon material to a continuous gas phase vapor deposition CVD furnace, and then introduce a mixed gas of acetylene and argon with a volume ratio of 4%:96%, and the temperature is increased to 800°C at a heating rate of 10°C / min. After keeping warm at 800°C for 1 hour, it is cooled to room temperature to obtain a lignin-based hard carbon composite material. The rest are consistent with the steps of Example 1, and the obtained battery material is tested by the same method as Example 1 (during the test preparation, the lignin-based hard carbon composite material replaces the bamboo-based and lignin-based hard carbon composite materials).
[0148] It should be noted that, in this embodiment, bamboo-based coated hard carbon is not prepared.
[0149] Comparative Example 7
[0150] A method for preparing a bamboo-based and lignin-based hard carbon composite material. Compared with Example 1, the difference lies in that: step S7 is to mix a bamboo-based soaking material and a lignin-based soaking material with a mass ratio of 3:7 with a phenolic resin at room temperature using a VC machine, wherein the mass of the phenolic resin is 5wt% of the total mass of the bamboo-based and lignin-based soaked materials; after mixing for 30 minutes, the mixture is put into a push plate furnace for high-temperature segmented carbonization; in a nitrogen atmosphere, the temperature is first increased to 800°C at a heating rate of 5°C / min and kept constant for 1 hour; then the temperature is increased to 1300°C at a heating rate of 2°C / min and kept constant for 3 hours; finally, the temperature is reduced to 800°C at a cooling rate of 4°C / min and then naturally cooled to 30°C to obtain a bamboo-based and lignin-based hard carbon composite material; there is no step 8, and the bamboo-based and lignin-based hard carbon composite material is prepared by step S9.
[0151] The rest of the steps are consistent with those in Example 1, and the obtained battery material is tested using the same method as in Example 1.
[0152] It should be noted that, in this embodiment, in step S7, bamboo-based coated hard carbon and lignin-based coated hard carbon are not prepared separately, but the bamboo-based soaking material and the lignin-based soaking material are mixed and used as raw materials to prepare bamboo-based and lignin-based hard carbon composite materials.
[0153] Comparative Example 8
[0154] A method for preparing a bamboo-based and lignin-based hard carbon composite material, compared with Example 1, the difference is that: there is no step S9, and the bamboo-based and lignin-based hard carbon mixture obtained in step S8 is used to prepare a sodium ion battery.
[0155] The rest of the steps are consistent with those in Example 1, and the obtained battery material is tested using the same method as in Example 1.
[0156] Comparative Example 9
[0157] A method for preparing a bamboo-based and lignin-based hard carbon composite material, compared with Example 1, the difference is that: step S9 carbon coating adopts VC mixed coating, and the rest are consistent with the steps of Example 1, and the obtained battery material is tested by the same method as Example 1.
[0158] The 21 bamboo-based and lignin-based hard carbon composite materials prepared in Examples 1-12 and Comparative Examples 1-9 were subjected to powder compaction density tests and assembled into sodium ion button batteries for electrochemical performance tests. The test results are shown in Tables 1 and Figure 1-2 shown.
[0159] Specific testing requirements:
[0160] Powder compaction density test: 5T powder is compacted using the powder compaction density meter PCD2000 and measured in accordance with the national standard GB / T24533-2019 powder compaction density.
[0161] Electrochemical performance test: The test was conducted using the Xinwei test system; test conditions: charge and discharge at a rate of 0.1C within a voltage range of 0 to 2V.
[0162] Table 1 Electrochemical performance of sodium ion batteries
[0163]
[0164]
[0165] According to the test results of Examples 1-12 in Table 1, the present invention uses bamboo-based or lignin as biomass raw materials, which are pretreated with an acidic oxidant, first pre-oxidized and then pre-carbonized, then pickled and soaked, and then coated with high-temperature segmented carbonization. Finally, the bamboo-based and lignin-based coated carbonized materials are mixed to prepare bamboo-based and lignin-based hard carbon composite materials having high sodium storage capacity and compaction density.
[0166] Compared with Example 1, in Examples 2 and 3, the concentrations of formic acid and H2O2 in Example 3 are reduced, while those in Example 2 are increased. The increased concentrations of formic acid and H2O2 make the connection between cellulose, lignin and hemicellulose more thoroughly destroyed, and the components more fully separated, which is beneficial to improve the carbon yield after subsequent acid washing, impurity removal and carbonization, thereby greatly improving the reversible specific capacity and compacted density, and ultimately improving the first coulombic efficiency, specific capacity and energy density.
[0167] In Example 4 compared with Example 1, the pre-oxidation temperature is relatively low, so that the introduced oxygen-containing, hydroxyl and carbonyl functional groups cannot produce a good cross-linking effect with the cellulose molecules, a large amount of disordered structures are not produced, and few nanopores are produced, which makes the capacity and compaction density of the hard carbon composite material relatively low.
[0168] In Example 5, compared with Example 1, the particle size of the crushed material becomes larger, the flowability and compressibility of the powder particles become worse, the powder particles are not packed tightly, the porosity between the powders is large, which reduces the compaction density and ultimately leads to a low capacity of the hard carbon material.
[0169] Example 6 Compared with Example 1, the concentration of phosphoric acid increased, which not only further dissolved and decrystallized cellulose, hemicellulose and lignin, but also introduced more doped P, which enhanced the reaction activity. + The number of storage sites increases, and the conductivity and wettability are improved, thereby increasing the specific capacity of the hard carbon negative electrode material.
[0170] Compared with Example 1, Examples 7 and 8 use different contents of modifiers to coat the bamboo-based and lignin-based materials after soaking, and Examples 9, 10, 11, and 12 use different composite ratios compared with Example 1. Due to the different hard carbon precursors, their internal microstructures, pore sizes, pore structures, surface areas, and surface functional groups are different, which makes the optimal ratios of high-temperature coating carbonization and composite after coating carbonization inconsistent. Separately coating and carbonizing the precursors can make the coating more uniform and denser, and the composite hard carbon materials after coating and carbonization can produce a synergistic effect to exert their respective advantages, thereby maintaining both the high capacity of the bamboo base and the high compaction of the lignin base.
[0171] According to Table 1, compared with Examples 1-12, the bamboo-based and lignin-based hard carbon composite materials in Comparative Example 1 are not pretreated with acidic oxidants, and the connections between cellulose, lignin and hemicellulose in the biomass raw materials are mostly not destroyed, and the separation of the components is not well achieved, which is not conducive to the subsequent acid washing and impurity removal and the utilization rate of the raw materials, thereby reducing the active sites of the hard carbon composite materials, reducing the interlayer spacing, and ultimately reducing the initial coulombic efficiency, specific capacity and compaction density.
[0172] According to Table 1, compared with Examples 1-12, the bamboo-based and lignin-based hard carbon composite materials in Comparative Example 2 were not pre-oxidized, and the lignocellulose hard carbon materials obtained by direct carbonization exhibited poor electrochemical properties due to relatively low conductivity and cross-linking degree and fewer sodium ion storage sites.
[0173] According to Table 1, compared with Examples 1-12, the bamboo-based and lignin-based hard carbon composite materials in Comparative Example 3 did not undergo a phosphoric acid soaking process, did not further dissolve and decrystallize cellulose, hemicellulose and lignin, and did not introduce P element doping, which resulted in reduced reaction activity, fewer storage sites, reduced conductivity and wettability, and thus reduced specific capacity of the hard carbon composite material.
[0174] According to Table 1, compared with Examples 1-12, the bamboo-based and lignin-based hard carbon composite materials in Comparative Example 4 change the high-temperature segmented carbonization to a one-step high-temperature carbonization, and the release of organic molecules is insufficient, which is not conducive to the formation of a rich pore structure; it also cannot increase the degree of graphitization and expand the interlayer spacing, which is not conducive to the embedding and removal of sodium ions in the material, thereby resulting in reduced capacity, first coulomb efficiency and compaction density.
[0175] According to Table 1, compared with Examples 1-12, in Comparative Examples 5 and 6, the bamboo-based and lignin-based hard carbon materials are not compounded, so that a synergistic effect cannot be produced to give full play to their respective advantages, and both the high capacity of the bamboo-based and the high compaction of the lignin-based cannot be maintained.
[0176] According to Table 1 and Figure 2 Compared with Examples 1-12, the bamboo-based and lignin-based hard carbon composite materials in Comparative Example 7 are first mixed and then coated and carbonized. Because the hard carbon precursors are different, their internal microstructures, pore sizes, pore structures, surface areas and surface functional groups are different, which makes the optimal coating ratio inconsistent, resulting in uneven and non-dense coating of the mixed materials, and cannot give full play to their respective advantages, so that it can maintain both the high capacity of the bamboo-based and the high compaction of the lignin-based.
[0177] According to Table 1, compared with Examples 1-12, Comparative Examples 8 and 9 have no CVD coating, while Comparative Example 9 uses VC mixed coating. Due to the uneven and non-dense coating, the conductivity of the composite material is poor, resulting in low capacity and compaction.
[0178] according to Figure 1 , showing two obvious characteristic peaks in the range of 25°~30° and 45°~50°, corresponding to the (002) crystal plane and the (101) crystal plane, respectively, indicating that the composite materials of Comparative Example 1 and Example 1 are bamboo-based and lignin-based hard carbon composite materials.
[0179] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention is described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing bamboo-based coated hard carbon, characterized in that: The following steps are included: Pre-treating the raw material to obtain a pre-treated material; The raw material comprises bamboo-based biomass raw material; The pretreated material is pretreated with an acidic oxidant to obtain an acidic oxidant pretreated material; pre-oxidizing the acidic oxidant pretreated material to obtain a pre-oxidized material; Pre-carbonizing the pre-oxidized material under a protective atmosphere to obtain a pre-carbonized material; crushing the pre-carbonized material to obtain a crushed material; The crushed material is firstly acid-washed and then water-washed to obtain a purified material; The purified material is soaked in acid, filtered and dried to obtain a soaked material; the acid for the acid soaking includes phosphoric acid; The soaked material is mixed evenly with the modifier, and then high-temperature coating and carbonization are carried out under a protective atmosphere to obtain bamboo-based coated hard carbon.
2. A method for preparing lignin-based hard carbon, characterized in that: The following steps are included: Pre-treating the raw material to obtain a pre-treated material; The feedstock comprises a lignin-based biomass feedstock; The pretreated material is pretreated with an acidic oxidant to obtain an acidic oxidant pretreated material; pre-oxidizing the acidic oxidant pretreated material to obtain a pre-oxidized material; Pre-carbonizing the pre-oxidized material under a protective atmosphere to obtain a pre-carbonized material; The pre-carbonized material is crushed to obtain a crushed material; The crushed material is firstly acid-washed and then water-washed to obtain a purified material; The purified material is soaked in acid, filtered and dried to obtain a soaked material; the acid for the acid soaking includes phosphoric acid; The soaked material is mixed evenly with the modifier, and then subjected to high-temperature coating and carbonization under a protective atmosphere to obtain lignin-based coated hard carbon.
3. A method for preparing a bamboo-based and lignin-based hard carbon composite material, characterized in that: The method comprises the following steps: preparing bamboo-based coated hard carbon and lignin-based coated hard carbon respectively, mixing the bamboo-based coated hard carbon and the lignin-based coated hard carbon, and then carbon coating the mixture to obtain a bamboo-based and lignin-based hard carbon composite material; The bamboo-based coated hard carbon is prepared by the method for preparing bamboo-based coated hard carbon according to claim 1; The lignin-based coated hard carbon is prepared by the preparation method of lignin-based coated hard carbon described in claim 2.
4. The method for preparing the bamboo-based and lignin-based hard carbon composite material according to claim 3, characterized in that: The raw material comprises at least one of bamboo and wood; When preparing bamboo-based coated hard carbon and lignin-based coated hard carbon, the pretreatment parameters include: washing the raw materials with water, and then drying them in a drying oven, the drying temperature of the drying oven is 60-120° C., and the drying time is 4-24 hours.
5. The method for preparing the bamboo-based and lignin-based hard carbon composite material according to claim 3, characterized in that: When preparing bamboo-based coated hard carbon and lignin-based coated hard carbon, the parameters of pre-treating the pre-treated material with an acidic oxidant include: reacting the pre-treated material with the acidic oxidant at 60-100° C. for 4-12 hours, the acidic oxidant includes an oxidant and an acid, wherein the oxidant includes at least one of hydrogen peroxide, peracetic acid, and ozone, the concentration of the oxidant is 1-5%, the acid includes at least one of formic acid and acetic acid, the concentration of the acid is 0.5-2%, and the solid-liquid mass ratio of the pre-treated material to the acidic oxidant is 1:1.2-5; When preparing bamboo-based coated hard carbon and lignin-based coated hard carbon, the acidic oxidant pretreated material is preoxidized, and the parameters of the preoxidized material include: temperature of 200-350° C., and preoxidation time of 3-5 hours.
6. The method for preparing the bamboo-based and lignin-based hard carbon composite material according to claim 3, characterized in that: When preparing bamboo-based coated hard carbon and lignin-based coated hard carbon, the pre-oxidized material is pre-carbonized under a protective atmosphere, and the parameters of the pre-carbonized material include: a heating rate of 2 to 10°C / min, a pre-carbonization temperature of 200 to 800°C, and a holding time of 1 to 3h. The pre-carbonization is carried out in a rotary kiln, and the protective atmosphere includes at least one of nitrogen, argon, and helium. When preparing bamboo-based coated hard carbon and lignin-based coated hard carbon, the pre-carbonized material is crushed, and the parameters of the crushed material include: the equipment used for the crushing includes at least one of a mechanical crusher, a roller mill crusher, and a jet mill, and the particle size D50 of the crushed material is controlled at 3 to 10 um.
7. The method for preparing the bamboo-based and lignin-based hard carbon composite material according to claim 3, characterized in that: When preparing bamboo-based coated hard carbon and lignin-based coated hard carbon, the crushed material is firstly acid-washed and then water-washed, and the parameters of the purified material include: the acid for acid washing includes at least two of hydrochloric acid, nitric acid, hydrofluoric acid and sulfuric acid; the acid concentration of the acid washing is 20-50%, the reaction temperature of the acid washing is 60-100°C, the solid-liquid mass ratio of the acid washing is 1:0.7-5.5, and the acid washing time is 4-24h; the water washing process includes: multiple deionized water washing until the filtrate is close to neutral, and then suction filtration and drying, the drying temperature is 60-120°C, and the drying time is 6-24h; When preparing bamboo-based coated hard carbon and lignin-based coated hard carbon, the purified material is soaked in a phosphoric acid solution, and the parameters of the soaked material include: the concentration of the phosphoric acid is 3-30%, the soaking time is 3-24 hours, and the solid-liquid mass ratio is 1:1.2-3; stirring is performed while soaking, and after soaking, the material is filtered and dried at a temperature of 60-120°C and a drying time of 4-24 hours; when preparing bamboo-based coated hard carbon and lignin-based coated hard carbon, the soaked material is evenly mixed with a modifier, and then the parameters of high-temperature coating carbonization are performed under a protective atmosphere, and the modifier includes: the modifier includes at least one of asphalt and resin, and the mass of the modifier accounts for 1-10wt% of the mass of the soaked material; the mixing time is 0.5-3h; High-temperature coating carbonization is high-temperature segmented carbonization: the first stage is low-temperature carbonization, the temperature is 800-1000℃, the heating rate is 4-6℃ / min, and the constant temperature time is 1-2h; the second stage is high-temperature carbonization, the temperature is 1200-1400℃, the heating rate is 1-2℃ / min, and the constant temperature time is 2-4h; the third stage is cooling, cooling to 800-1100℃, the cooling rate is 3-5℃ / min, and the protective atmosphere is continued to cool naturally to 25-30℃; The protective atmosphere includes at least one of nitrogen, argon and helium.
8. The method for preparing the bamboo-based and lignin-based hard carbon composite material according to claim 3, characterized in that: When the bamboo-based coated hard carbon and the lignin-based coated hard carbon are mixed and then carbon-coated to obtain a bamboo-based and lignin-based hard carbon composite material, the bamboo-based coated hard carbon and the lignin-based coated hard carbon are mixed and then added to a CVD carbon coating device, and then a carbon source and a protective gas are introduced, the temperature is increased, the temperature is kept, and the temperature is cooled to obtain a bamboo-based and lignin-based hard carbon composite material; Among them, the mass ratio of the bamboo-based coated hard carbon and the lignin-based coated hard carbon is 1:9-9:1, the mixing time is 0.5-2h, the carbon source includes at least one of acetylene, methane, propane, ethylene, propylene, and benzene, the protective gas includes at least one of argon and nitrogen, the volume fraction of the carbon source and the protective gas is 4%-10%:96%-90%, the heating rate is 5-10℃ / min, the heating temperature is 650-1000℃, and the insulation time is 0.5-4h; the CVD carbon coating equipment includes at least one of a CVD rotary furnace, an intermittent vapor deposition CVD furnace, and a continuous vapor deposition CVD furnace.
9. A negative electrode plate, characterized in that: The negative electrode plate uses bamboo-based and lignin-based hard carbon composite materials as active materials for the battery negative electrode material, and the bamboo-based and lignin-based hard carbon composite materials are prepared by the preparation method of the bamboo-based and lignin-based hard carbon composite materials described in any one of claims 3 to 8.
10. A battery, characterized in that: This battery is a sodium ion battery, which includes a negative electrode, a positive electrode, a separator, and an electrolyte. The negative electrode includes the negative electrode plate according to claim 9. A charge and discharge test is performed at a current density of 0.1C. The first charge specific capacity of the sodium ion battery is greater than 330mAh / g, and the first coulomb efficiency is greater than 90%.
Citation Information
Patent Citations
Hard carbon negative electrode material, preparation method thereof and battery containing hard carbon negative electrode material
CN114804068A
Reed-derived hard carbon sodium battery negative electrode material, preparation method thereof and energy storage battery
CN115528232A
Bamboo-based hard carbon material, preparation thereof and application of bamboo-based hard carbon material in sodium ion battery
CN117105199A
Moso bamboo biomass hard carbon production and manufacturing technology
CN117534055A
High-rate biomass-based hard carbon negative electrode material and preparation method thereof
CN117963885A
Cited By
Biomass-based hard carbon material, preparation method thereof and battery
CN119735194A
Element-doped biomass hard carbon negative electrode material and preparation method thereof
CN120622464A
Preparation method of sodium electric hard carbon material
CN120622466A
A method for preparing a sodium hard carbon material
CN120622466B
Preparation method of high-rate long-cycle hard carbon negative electrode, negative electrode and battery
CN120854490A