Method for charging non-aqueous electrolyte secondary battery

The charging method for lithium-rich secondary batteries addresses instability by managing hysteresis characteristics through controlled voltage transitions, achieving high capacity and durability by stabilizing oxygen species formation.

JP7576744B2Active Publication Date: 2024-11-01PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022503703
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-27
Filing Date
2021-02-25
Publication Date
2024-11-01
Estimated Expiration
2041-02-25

AI Technical Summary

Technical Problem

Lithium-rich positive electrode active materials in secondary batteries suffer from instability and reduced durability due to the formation of unstable oxygen species during high-voltage charging, leading to capacity degradation over repeated cycles.

Method used

A charging method involving constant current charging to a predetermined voltage V2 higher than V1, followed by constant current discharging to a lower voltage V3, where V3 < V1 < V2, to manage hysteresis characteristics and stabilize the battery, ensuring 0.99C1 ≦ C3 < C2, thereby maintaining high capacity and durability.

Benefits of technology

The method enhances battery capacity and durability by suppressing the formation of unstable oxygen species, allowing for increased capacity retention and improved stability during charging and discharging cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576744000002
    Figure 0007576744000002
  • Figure 0007576744000003
    Figure 0007576744000003
  • Figure 0007576744000004
    Figure 0007576744000004
Patent Text Reader

Abstract

This charging method is a method for charging a nonaqueous electrolyte secondary cell containing a lithium-rich positive-electrode active material. When constant-current charging is performed to a predetermined voltage V2 which is equal to or higher than a setting voltage V1, and then constant-current discharging is performed to a predetermined voltage V3, V3<V1≤V2 is satisfied. Cell capacity C1 at V1, cell capacity C2 at V2, and cell capacity C3 at V3 satisfy 0.99C1≤C3<C2.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a method for charging a non-aqueous electrolyte secondary battery, and more particularly to a method for charging a non-aqueous electrolyte secondary battery that includes an excess lithium type positive electrode active material. [Background technology]

[0002] Lithium transition metal composite oxides have been widely used as positive electrode active materials for secondary batteries such as lithium ion batteries, and lithium-rich positive electrode active materials that contain a large amount of lithium have been attracting attention as materials for high-capacity secondary batteries. Patent Document 1 discloses a charging method in which constant current charging is followed by constant voltage charging in order to achieve good discharge capacity and a short initial charging time while suppressing swelling of a battery that contains a lithium-rich positive electrode active material. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-61874 A Summary of the Invention

[0004] In positive electrodes that contain lithium-excess positive electrode active materials, the redox of not only transition metals but also anions such as oxygen is utilized, so there is unstable oxygen (O - ) may exist. This tendency becomes more pronounced after charging to a certain high voltage or higher, and the positive electrode and electrolyte are prone to deterioration. Since secondary batteries are used by repeatedly charging and discharging, if they are held at a high potential each time they are charged, the battery deteriorates and its durability deteriorates. The charging method disclosed in Patent Document 1 still has room for improvement in terms of battery durability.

[0005] One aspect of the present disclosure is a charging method for a non-aqueous electrolyte secondary battery including a lithium-excess type positive electrode active material. After constant current charging to a predetermined voltage V2 equal to or higher than a set voltage V1, constant current discharging is performed to a predetermined voltage V3, where V3 < V1 ≤ V2, and the battery capacity C1 at V1, the battery capacity C2 at V2, and the battery capacity C3 at V3 satisfy 0.99C1 ≤ C3 < C2.

[0006] According to the charging method which is one aspect of the present disclosure, it is possible to achieve both high capacity and high durability in a non-aqueous electrolyte secondary battery.

Brief Description of the Drawings

[0007] [Figure 1] FIG. 1 is a configuration block diagram of a secondary battery and a charge / discharge control device in an example of the embodiment. [Diagram 2] FIG. 2 is a diagram showing a charging method which is an example of the embodiment. [Diagram 3] FIG. 3 is a diagram showing a charging method which is another example of the embodiment. [Figure 4] FIG. 4 is a processing flowchart of the charging method shown in FIG. 2.

Embodiments for Carrying Out the Invention

[0008] First, the basic principle of the present embodiment will be described. Conventionally, when charging a secondary battery, a method of performing constant current charging and stopping the charging when the set voltage is reached has been used. However, when charging a secondary battery using a positive electrode containing a lithium-excess type positive electrode active material up to a high voltage state where the set voltage exceeds 4V with respect to the lithium electrode reference, unstable oxygen (O -) occurs, deteriorating the positive electrode and the electrolyte, and thus the battery capacity decreases due to repeated charge and discharge. As a result of intensive studies on such problems, the inventors of the present invention have noted that in the charge and discharge of a secondary battery containing a lithium-excess type positive electrode active material, the hysteresis characteristics of the voltage (V) with respect to the battery capacity (mAh / g) are larger than those of other NCA (Ni-Co-Al) based positive electrode active materials, etc., and have come up with a charging method in the following-described embodiment that can achieve both high capacity and high durability.

[0009] A charging method according to one embodiment of the present disclosure is a charging method for a non-aqueous electrolyte secondary battery containing a lithium-excess type positive electrode active material. After constant current charging to a predetermined voltage V2 equal to or higher than a set voltage V1, constant current discharging is performed to a predetermined voltage V3, where V3 < V1 ≤ V2, and the battery capacity C1 at V1, the battery capacity C2 at V2, and the battery capacity C3 at V3 satisfy 0.99C1 ≤ C3 < C2.

[0010] Next, the configuration of the present embodiment will be described. FIG. 1 is a configuration block diagram of a secondary battery 10 and a charge and discharge control device 12 in an example of the embodiment.

[0011] The secondary battery 10 is a lithium-ion secondary battery in which charge and discharge are performed by the movement of lithium ions through a non-aqueous electrolyte between a positive electrode and a negative electrode, and includes a positive electrode having a positive electrode mixture layer containing a positive electrode active material and a negative electrode having a negative electrode mixture layer containing a negative electrode active material. The outer shape of the secondary battery 10 is not particularly limited, and may be, for example, cylindrical, rectangular, coin-shaped, etc., or may be a battery case composed of a laminate sheet including a metal layer and a resin layer.

[0012] The positive electrode included in the secondary battery 10 is composed of, for example, a positive electrode current collector such as a metal foil, and a positive electrode mixture layer formed on the positive electrode current collector. As the positive electrode current collector, a foil of a metal stable within the potential range of the positive electrode such as aluminum, a film having the metal disposed on the surface layer, or the like can be used. The positive electrode mixture layer contains, for example, a positive electrode active material, a binder, a conductive agent, and the like. The positive electrode can be manufactured, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a binder, a conductive agent, etc. onto the positive electrode current collector, drying to form the positive electrode mixture layer, and then rolling this positive electrode mixture layer.

[0013] As the positive electrode active material, a lithium-excess type positive electrode active material is used. The lithium-excess type positive electrode active material has the general formula Li x Mn y Ni z Me 2-x-y-z O a F b (where 1 ≤ x ≤ 1.2, 0.4 ≤ y ≤ 0.8, 0 ≤ z ≤ 0.4, 0 < b ≤ 0.2, 1.9 ≤ a + b ≤ 2.1, and Me is at least one element selected from Co, Ti, Al, Si, Sr, Nb, W, Mo, P, Ca, Mg, Sb, Na, B, V, Cr, Fe, Cu, Zn, Ge, Zr, Ru, K, and Bi). The secondary battery 10 containing the lithium-excess type positive electrode active material has a larger voltage hysteresis characteristic with respect to the battery capacity in charge and discharge compared to other NCA (Ni-Co-Al) based positive electrode active materials and the like. Therefore, if the charging method, which is one aspect of the present disclosure described later, is used, high capacity and high durability can be achieved simultaneously.

[0014] Examples of the conductive agent include carbon-based particles such as carbon black (CB), acetylene black (AB), ketjen black, and graphite. These may be used alone or in combination of two or more. Examples of the binder include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide-based resins, acrylic resins, and polyolefin-based resins. These may be used alone or in combination of two or more.

[0015] The negative electrode included in the secondary battery 10 includes a negative electrode current collector such as a metal foil, and a negative electrode mixture layer formed on the negative electrode current collector. For the negative electrode current collector, a foil of a metal such as copper that is stable in the potential range of the negative electrode, or a film with the metal disposed on the surface layer, can be used. The negative electrode mixture layer includes, for example, a negative electrode active material, a thickener, a binder, etc. The negative electrode can be produced, for example, by applying a negative electrode mixture slurry including a negative electrode active material, a thickener, a binder, etc., onto the negative electrode current collector, drying the slurry to form a negative electrode mixture layer, and then rolling the negative electrode mixture layer.

[0016] The negative electrode active material is not particularly limited as long as it is a material capable of absorbing and releasing lithium ions, and may be, for example, a carbon material such as graphite, non-graphitizable carbon, graphitizable carbon, fibrous carbon, coke, carbon black, etc. Also, for example, a non-carbon material such as silicon, tin, and alloys and oxides mainly containing these may be used as the negative electrode active material.

[0017] As the binder, for example, PTFE or the like may be used as in the case of the positive electrode, or styrene-butadiene copolymer (SBR) or a modified product thereof may be used. As the thickener, for example, carboxymethylcellulose (CMC) or a modified product thereof (including salts such as Na salt) may be used.

[0018] The non-aqueous electrolyte contained in the secondary battery 10 includes a non-aqueous solvent and an electrolyte salt. As the non-aqueous solvent (organic solvent), for example, carbonates, lactones, ethers, ketones, esters, etc. can be used, and two or more of these solvents can be mixed and used. As the electrolyte salt, for example, LiPF6, LiBF4, LiCF3SO3, etc., and mixtures thereof can be used. The amount of electrolyte salt dissolved in the non-aqueous solvent can be, for example, 0.5 to 2.0 mol / L.

[0019] 1, a discharge / charge / discharge control device 12 controls charging and discharging of a secondary battery 10 while measuring the voltage, battery capacity, etc. of the secondary battery 10. The discharge / charge / discharge control device 12 includes a processor and a memory, and includes a measuring unit 120, a recording unit 122, and a control unit 124 as functional blocks.

[0020] The measurement unit 120 measures the voltage and battery capacity of the secondary battery 10. The measurement unit 120 may measure the time from the start of charging.

[0021] The recording unit 122 records the voltage and battery capacity of the secondary battery 10 measured by the measurement unit 120. The recording unit 122 may also record the time from the start of charging.

[0022] The control unit 124 controls the charging and discharging of the secondary battery 10. When the voltage of the secondary battery 10 measured by the measurement unit 120 reaches a predetermined voltage, the control unit 124 stops the constant current charging and starts the constant current discharging. After that, when the predetermined voltage is reached, the control unit 124 stops the constant current discharging.

[0023] Next, a specific charging method will be described below. Fig. 2 is a diagram showing a charging method according to an embodiment.

[0024] Before charging, the secondary battery 10 is in a state P0 with a constant voltage and a constant battery capacity. When constant current charging is started, the secondary battery 10 increases in battery capacity from state P0, and the voltage rises, reaching state P1. In state P1, the voltage is a set voltage V1 and the battery capacity is C1. In the vicinity of set voltage V1, oxygen (O - ) is likely to occur.

[0025] V1 may be 4.4 V or more based on the lithium electrode (hereinafter, the potential based on the lithium electrode may be expressed as vsLi). This increases the battery capacity C1, so that a secondary battery 10 with a large capacity (C3) and a reduced voltage (V3) can be obtained.

[0026] Next, even after reaching the set voltage V1, constant current charging is performed up to a predetermined voltage V2 that is equal to or higher than the set voltage V1, and the secondary battery 10 reaches the state of P2. In the state of P2, the battery capacity is C2.

[0027] V2 may be 4.9 V or less based on the lithium electrode reference. When V2 > 4.9 V vs Li, damage may remain in the positive electrode and the electrolyte, and the durability may deteriorate.

[0028] Furthermore, constant current discharging is performed up to a predetermined voltage V3, and the secondary battery 10 reaches the state of P3. In the state of P3, the battery capacity is C3. From the above relationship, V1, V2, and V3 satisfy V3 < V1 < V2. Since V3 < V1, the secondary battery 10 in the state of P3 can suppress the generation of unstable oxygen (O - ) better than the secondary battery 10 in the state of P1. It is preferable to start constant current discharging as soon as possible after the secondary battery 10 reaches the state of P2. The holding time in the state of P2 may be, for example, 1 minute or less, preferably 30 seconds or less, and more preferably 10 seconds or less.

[0029] Also, in the charge and discharge of a secondary battery containing a lithium-excess type positive electrode active material, since the voltage with respect to the battery capacity has a relatively large hysteresis, the battery capacity C3 of the secondary battery 10 in the state of P3 can be made substantially equal to or greater than the battery capacity C1 of the secondary battery 10 in the state of P1. In other words, C1, C2, and C3 can satisfy 0.99C1 ≦ C3 < C2. Thereby, while increasing the battery capacity of the secondary battery 10 at the end of charging (state of P3), the voltage can be lowered, so the durability of the battery is improved.

[0030] C3 is preferably 90% SOC or more, and more preferably 95% SOC or more. The closer the secondary battery 10 is to full charge at the end of charging (state of P3), the more significant the above effects become.

[0031] FIG. 3 is a diagram showing a charging method which is another example of the embodiment.

[0032] Before charging, the secondary battery 10 is in the state of P0 having a constant voltage and a constant battery capacity as shown in FIG. 2. By constant current charging, the voltage reaches the state of P1 with the set voltage V1 and the battery capacity C1. Near the set voltage V1, oxygen (O - ) is likely to be generated due to the high voltage. In the method illustrated in FIG. 3, different from the case of FIG. 2, instead of constant current charging from the set voltage V1 to V2, constant current discharging is performed up to a predetermined voltage V3, and the secondary battery 10 reaches the state of P3. That is, V1, V2, and V3 satisfy V3 < V1 = V2. Since V3 < V1, the secondary battery 10 in the state of P3 can suppress the generation of unstable oxygen (O - ) compared to the secondary battery 10 in the state of P1. Here, 4.4V vs Li ≤ V1(V2) ≤ 4.9V vs Li may be satisfied.

[0033] Also, in the method illustrated in FIG. 3, similar to the case of FIG. 2, C1, C2, and C3 can be made to satisfy 0.99C1(C2) ≤ C3 < C1(C2). Thereby, while increasing the battery capacity of the secondary battery 10 at the end of charging (state of P3), the voltage can be lowered, so the durability of the battery is improved. Here, C3 is preferably 90% SOC or more, and more preferably 95% SOC or more.

[0034] FIG. 4 is a processing flowchart of the charging method shown in FIG. 2.

[0035] First, while the measurement unit 120 measures the voltage and the battery capacity, the control unit 124 performs constant current charging of the secondary battery 10 up to the set voltage V1 (S100). Also, the battery capacity C1 when the secondary battery 10 reaches the voltage V1 is recorded in the recording unit 122 (S102). At the same time, the time t1 from the start of charging may be recorded in the recording unit 122.

[0036] Furthermore, while the measurement unit 120 measures the voltage and the battery capacity, the control unit 124 performs constant current charging of the secondary battery 10 up to a predetermined voltage V2 (S104). Also, the battery capacity C2 when the secondary battery 10 reaches the voltage V2 is recorded in the recording unit 122 (S106). At the same time, the time t2 from the start of charging may be recorded in the recording unit 122.

[0037] Thereafter, the control unit 124 discharges the secondary battery 10 at a constant current to a predetermined voltage V3 (S108) while the measurement unit 120 measures the voltage and battery capacity. In addition, the battery capacity C3 when the secondary battery 10 reaches the voltage V3 is recorded in the recording unit 122 (S110). At the same time, the time t3 from the start of charging may be recorded in the recording unit 122.

[0038] Through the above steps, the secondary battery 10 in the P3 state is obtained. After the secondary battery 10 in the P3 state is used (discharged) and returns to the initial P0 state, the above steps can be performed again to obtain the secondary battery 10 in the P3 state. At this time, instead of measuring the voltage and battery capacity by the measuring unit 120, the secondary battery 10 may be charged using t1, t2, and t3 recorded in the recording unit 122.

[0039] The charging method shown in FIG. 3 can also be processed according to a flowchart similar to that shown in FIG.

[0040] <Example> The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.

[0041] <Example 1> [Preparation of positive electrode] General formula Li 1.1166 Mn 0.556 Ni 0.278 O 1.94 F 0.06 A positive electrode active material having a composition represented by the formula (I), acetylene black, and polyvinylidene fluoride (PVdF) were mixed in a mass ratio of 92:5:3, and N-methyl-2-pyrrolidone (NMP) was used as a dispersion medium to prepare a positive electrode mixture slurry. Next, this positive electrode mixture slurry was applied to the surface of a positive electrode core made of aluminum foil, and the coating was dried and compressed, and then cut into a predetermined electrode size to produce a positive electrode in which a positive electrode mixture layer was formed on the positive electrode core.

[0042] [Preparation of non-aqueous electrolyte] A non-aqueous electrolyte was prepared by dissolving LiPF6 at a concentration of 1 mol / L in a mixed solvent in which fluoroethylene carbonate (FEC) and methyl 3,3,3-trifluoropropionate (FMP) were mixed in a mass ratio of 1:3.

[0043] [Preparation of test cell] Lead wires were attached to the positive electrode and the counter electrode made of Li metal, and the positive electrode and the counter electrode were arranged opposite each other via a polyolefin separator to prepare an electrode body. This electrode body and the non-aqueous electrolyte were enclosed in an exterior body made of an aluminum laminate film to prepare a test cell. The test cell was charged at a constant current of 0.5 It in a temperature environment of 25°C until the battery voltage reached 3.0 V vs Li (V0), and this state was designated as the initial state.

[0044] [Evaluation of energy density retention rate after cycle testing] The following cycle test was performed on the test cell in the initial state described above. The discharge capacity at the first cycle and the discharge capacity at the 25th cycle of the cycle test were obtained, and the capacity retention rate was calculated using the following formula. The capacity retention rate was multiplied by the average voltage during discharge, V ave The energy density maintenance rate was calculated by multiplying the result by

[0045] Capacity retention rate (%) = (25th cycle discharge capacity ÷ 1st cycle discharge capacity) × 100 Energy density retention rate (%) = Capacity retention rate × Average voltage V ave <Cycle test> First, the initial test cell was charged at a constant current in a temperature environment of 25°C until the battery voltage reached 4.75VvsLi (V2), which was higher than the set voltage of 4.7VvsLi (V1), and then discharged at a constant current of 0.5It until the battery voltage reached 4.5VvsLi. After that, the test cell was discharged at a constant current of 1It until the battery voltage reached 3.0VvsLi (V0). This charge / discharge cycle was repeated 25 times.

[0046] <Examples 2 to 4> The test cells were evaluated in the same manner as in Example 1, except that V1, V2, and V3 were changed as shown in Table 1.

[0047] <Comparative Example 1> The battery was charged at a constant current until the battery voltage reached a set voltage of 4.7 V vs Li (V1). Then, the battery was discharged at a constant current of 1 It until the battery voltage reached 3.0 V vs Li (V0). This charge / discharge cycle was repeated 25 times.

[0048] <Comparative Example 2> The test cell was evaluated in the same manner as in Comparative Example 1, except that V1 was changed to 4.6 V vs Li.

[0049] The results of the energy density retention rates of the test cells of the Examples and Comparative Examples are summarized in Table 1. The energy density retention rates of Examples 1 and 2 are shown as relative values ​​with the energy density retention rate of Comparative Example 1 set to 100, and the energy density retention rates of Examples 3 and 4 are shown as relative values ​​with the energy density retention rate of Comparative Example 2 set to 100. Table 1 also shows the voltages (V1, V2, V3) and battery capacities (C1, C2, C3) of the test cells in the states of P1, P2, and P3 of the Examples and Comparative Examples.

[0050] [Table 1]

[0051] The test cells of Examples 1 and 2 had a higher energy density retention rate than the test cell of Comparative Example 1, and the test cells of Examples 3 and 4 had a higher energy density retention rate than the test cell of Comparative Example 2. [Explanation of symbols]

[0052] 10 Secondary battery 12 Discharge / charge control device 120 Measurement section 122 Recording Section 124 Control Unit

Claims

1. A method for charging a non-aqueous electrolyte secondary battery including a lithium-excess positive electrode active material, comprising: After charging with a constant current to a predetermined voltage V2 that is equal to or higher than the set voltage V1, the battery is discharged with a constant current to a predetermined voltage V3. V3<V1≦V2, A charging method in which a battery capacity C1 at V1, a battery capacity C2 at V2, and a battery capacity C3 at V3 satisfy 0.99C1≦C3<C2.

2. The lithium-excess positive electrode active material is represented by the general formula Li x Mn y Ni z Me 2-x-y-z O a F b 2. The charging method according to claim 1, comprising a lithium transition metal composite oxide represented by the formula: (wherein 1≦x≦1.2, 0.4≦y≦0.8, 0≦z≦0.4, 0<b≦0.2, 1.9≦a+b≦2.1, and Me is at least one element selected from Co, Ti, Al, Si, Sr, Nb, W, Mo, P, Ca, Mg, Sb, Na, B, V, Cr, Fe, Cu, Zn, Ge, Zr, Ru, K, and Bi).

3. 3. The charging method according to claim 1 or 2, wherein V1 is 4.4 V or more based on the lithium electrode.

4. The charging method according to any one of claims 1 to 3, wherein V2 is 4.9 V or less based on the lithium electrode.

5. The charging method according to any one of claims 1 to 4, wherein C3 is SOC 90% or more.

Citation Information

Patent Citations

  • Battery control method for generator type electric automobile

    JP2000261905A

  • Positive electrode active material for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, battery pack, and method for producing positive electrode active material for nonaqueous electrolyte secondary battery

    JP2012089470A

  • Power storage system for fixation

    JP2017011849A

  • Charge rate estimating device

    JP2018136157A

  • Method of manufacturing power storage element

    JP2019061874A