Additive for imparting ultraviolet absorbing ability and / or high refractive index to a matrix and resin member using the same

Sulfur-containing additives integrated into ultraviolet absorbing skeletons improve compatibility and heat resistance, enabling high concentration use in resins to maintain transparency and enhance ultraviolet absorption and refractive index, addressing the limitations of conventional organic absorbers.

JP7576807B2Active Publication Date: 2024-11-01MIYOSHI OIL & FAT +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023107768
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2014-08-05
Filing Date
2023-06-30
Publication Date
2024-11-01
Estimated Expiration
2035-08-05

AI Technical Summary

Technical Problem

Conventional organic ultraviolet absorbers have limited compatibility with matrix resins, leading to difficulty in achieving high concentrations without clouding, and they often thermally decompose during resin processing, compromising transparency and ultraviolet absorption ability.

Method used

Development of additives represented by specific sulfur-containing groups integrated into benzotriazole, benzophenone, salicylate, or triazine ultraviolet absorbing skeletons, which enhance compatibility and heat resistance, allowing high concentration addition without loss of transparency and providing both ultraviolet absorption and high refractive index.

Benefits of technology

The additives maintain high transparency and exhibit excellent ultraviolet absorption and refractive index properties even at high concentrations, simplifying manufacturing processes and reducing costs by eliminating the need for separate layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007576807000078
    Figure 0007576807000078
  • Figure 0007576807000079
    Figure 0007576807000079
  • Figure 0007576807000080
    Figure 0007576807000080
Patent Text Reader

Abstract

To provide an additive for imparting ultraviolet absorptivity which has good compatibility to a resin as a matrix, or an additive for imparting a high refractive index.SOLUTION: An additive is represented by the following formula (III). In the formula, R1c to R10c are each independently a monovalent sulfur-containing group having a specific structure.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an additive for improving ultraviolet absorbing ability or adjusting the refractive index by adding it to a matrix such as a resin, and to a resin member using the additive.

[0002] 2. Description of the Related Art In optical materials such as optical films and optical molded products, it is important to impart optical functions such as ultraviolet absorption and refractive index adjustment, and various studies have been conducted on this matter.

[0003] Resin components deteriorate due to the action of ultraviolet rays, causing quality deterioration such as discoloration and reduced mechanical strength, which hinders long-term use. In order to prevent such quality deterioration or to control the wavelength of transmitted light, it is common to blend inorganic or organic ultraviolet absorbents into the resin components.

[0004] Inorganic ultraviolet absorbers have excellent durability such as weather resistance and heat resistance, but the absorption wavelength is determined by the band gap of the compound, so there is little freedom in selection, and few can absorb long-wave ultraviolet rays (UV-A, 315-400 nm) around 400 nm even among near ultraviolet rays, and those that absorb long-wave ultraviolet rays have absorption up to 450-500 nm (visible range), which results in coloring. Components used in solar cells, which have been developed in recent years, need to be exposed to sunlight outdoors for long periods of time, and their properties will inevitably deteriorate due to exposure to ultraviolet rays over a long period of time, so there is a demand for ultraviolet absorbers that have excellent light resistance, as well as durability against yellowing, etc., and show a shielding effect up to the UV-A range.

[0005] In contrast, organic ultraviolet absorbents have a high degree of freedom in the design of the absorbent structure, so that various absorption wavelengths can be obtained by devising the absorbent structure. On the other hand, when a resin composition containing an ultraviolet absorbent is heated to be molded or processed, the ultraviolet absorbent is thermally decomposed, which reduces the ultraviolet absorption ability of the resin member, and in the case of a transparent resin member, the transparency is impaired, and further, the inside of the molding or processing device may be contaminated, so that an organic ultraviolet absorbent with better heat resistance is required. Conventionally, as organic ultraviolet absorbents, ultraviolet absorbents such as benzotriazole-based, benzophenone-based, triazine-based, cyanoacrylate-based, and salicylate-based ones are known (see, for example, Patent Documents 1 to 4).

[0006] On the other hand, for optical films such as reflective films, anti-reflective films, and hard coat films, it is required to adjust the refractive index in order to adjust the optical properties. Conventionally, the refractive index is adjusted by adding a refractive index adjuster. As the refractive index adjuster, inorganic oxide fine particles and the like are used to increase the refractive index.

[0007] In addition, transparent resin members including optical molded products are desirably transparent after molding or over time in terms of their applications, and ultraviolet absorbents are required to prevent deterioration of optical properties caused by opacification or discoloration due to ultraviolet degradation. In particular, ultraviolet absorbents are required for eyeglass lenses and contact lenses from the viewpoint of protecting the eyes from ultraviolet rays.

[0008] In eyeglass lenses and the like, the refractive index of resins is becoming higher, and additives such as ultraviolet absorbers may have a lower refractive index than the resin. In such cases, the lower the refractive index of the additive and the more added, the lower the refractive index of the entire resin, so ultraviolet absorbers with a higher refractive index that can be added in high concentrations are required. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2012-184168 A [Patent Document 2] Special Publication No. 2005-504047 [Patent Document 3] JP 2013-67811 A [Patent Document 4] Special Publication No. 6-505744 Summary of the Invention [Problem to be solved by the invention]

[0010] However, many of the conventional organic ultraviolet absorbers have limitations in compatibility with the matrix resin, making it difficult to dissolve uniformly at high concentrations. When added at high concentrations, they cause cloudiness and impair transparency. Therefore, in applications requiring high transparency, there are limitations to the concentration in order to fully exhibit performance such as ultraviolet absorption ability and high refractive index. In addition, conventional organic ultraviolet absorbers may be thermally decomposed when a resin containing them is heated to be molded and processed, which impairs the ultraviolet absorption ability of the resulting resin member and the transparency of the transparent resin member, and there is a risk of contaminating the inside of the molding device.

[0011] In other words, there has been a demand for an additive that has excellent heat resistance, good compatibility with the matrix resin, and can be dissolved even in high concentrations so as to fully exhibit performance such as ultraviolet absorption and high refractive index while maintaining high transparency.

[0012] In addition, there are few studies on technology that allows one additive to provide both ultraviolet absorbing ability and high refractive index. For example, in the specific disclosures in Patent Documents 1 to 3, sulfur-containing compounds are not considered, and a high refractive index cannot be provided. Therefore, in the field of optical materials such as optical films, optical sheets, optical plates (plate-shaped members), and other optical molded products, for example, optical lenses such as lens elements for glasses, both ultraviolet absorbing ability and refractive index characteristics are often required, but in order to satisfy both of these requirements, an ultraviolet absorbing layer to which an ultraviolet absorbent is added and a high refractive index layer to which a refractive index adjuster is added are laminated as separate layers.

[0013] Patent Document 4 discloses a 5-thio-substituted benzotriazole ultraviolet absorber. This ultraviolet absorber provides a stabilized composition that protects organic substances against the harmful effects of exposure to ultraviolet light and suppresses deterioration over time, but no studies have been conducted focusing on the heat resistance, high refractive index, suitability for transparent resin matrices, compatibility (transparency) with the resin that becomes the matrix, suppression of yellowing of the resin matrix, increasing the refractive index of a resin member containing the ultraviolet absorber, deterioration of the ultraviolet absorption ability and appearance of the resin member due to thermal decomposition of the ultraviolet absorber, and further deterioration of transparency and suppression of yellowing in a transparent resin member.

[0014] The present invention has been made in consideration of the above circumstances, and has as its main object to provide an additive for imparting excellent heat resistance and ultraviolet absorption ability, or an additive for imparting a high refractive index, which has good compatibility with a matrix resin and can maintain high transparency even when added at a high concentration, and a resin part using the same.

[0015] Another object of the present invention is to provide an additive having excellent heat resistance that can exhibit both ultraviolet absorbing ability and high refractive index imparting ability while maintaining transparency, and a resin part using the additive. [Means for solving the problem]

[0016] In order to solve the above problems, the additive of the present invention is an additive for imparting ultraviolet absorbing ability and / or a high refractive index to a matrix, and has the following characteristics.

[0017] [1] An additive for imparting ultraviolet absorbing ability and / or a high refractive index to a matrix, represented by the following formula (I):

[0018] [ka]

[0019] (In the formula, R 1a ~R 9a each independently represents the following formula (i-1) or formula (i-2):

[0020] [ka]

[0021] (In formula (i-1), R 10a represents a divalent hydrocarbon group having 1 to 12 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, and m represents an integer of 0 or 1. In formula (i-2), R 11a represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom; R 12a When p is 2 or more, each independently represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, and R 13a represents a hydrogen atom or -(R 14a ) l -R 15a A group represented by R 14a represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, the terminal may be interrupted, or the carbon-carbon bond may be interrupted by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom; R 15arepresents a hydrogen atom or a substituent containing any one skeleton selected from benzotriazole, benzophenone, benzoic acid ester, and triazine. l represents an integer of 0 or 1. R 11a and p R 12a and R 13a has a total carbon number of 25 or less. n represents an integer of 0 or 1, and p represents an integer of 0 to 3. R represents a monovalent sulfur-containing group represented by the formula (I), a hydrogen atom, a monovalent hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a monovalent group selected from a halogen atom. 1a ~R 9a At least one of the groups is a monovalent sulfur-containing group represented by formula (i-1) or formula (i-2). [2] The additive according to [1], wherein the matrix is ​​a transparent resin.

[0022] [3] The monovalent sulfur-containing group is represented by formula (i-1), and the monovalent sulfur-containing group represented by formula (i-1) is a group in which m is 0 or m is 1 and R 10a The additive according to [1] or [2], wherein the alkylene group has 10 or less carbon atoms.

[0023] [4] The monovalent sulfur-containing group is represented by formula (i-1), and the monovalent sulfur-containing group represented by formula (i-1) is a group in which m is 0 or m is 1 and R 10a The additive according to [1] or [2], wherein the additive has an alkylene group having 9 or less carbon atoms and a melting point of 91° C. or less under normal pressure.

[0024] [5] The monovalent sulfur-containing group is represented by formula (i-1), and the monovalent sulfur-containing group represented by formula (i-1) is a group in which m is 0 or m is 1 and R 10a The additive according to [1] or [2], wherein the additive has an alkylene group having 8 or less carbon atoms and a melting point of less than 70° C. under normal pressure.

[0025] [6] The monovalent sulfur-containing group is represented by formula (i-1), and the monovalent sulfur-containing group represented by formula (i-1) is a group in which m is 0 or m is 1 and R10a The additive according to claim [1] or [2], wherein the additive has an alkylene group having 8 or less carbon atoms and a melting point of 35°C or less under normal pressure.

[0026] [7] The monovalent sulfur-containing group is represented by formula (i-1), and the monovalent sulfur-containing group represented by formula (i-1) is a group in which m is 0 or m is 1 and R 10a is an oxyalkylene group having 10 or less carbon atoms and an ether bond at a base end.

[0027] [8] The monovalent sulfur-containing group is represented by formula (i-2), and the monovalent sulfur-containing group represented by formula (i-2) is R 1a ~R 5a The additive according to [1] or [2], wherein the additive has the following structure at any one of the positions:

[0028] [9] The monovalent sulfur-containing group represented by formula (i-2) is R 11a and p R 12a and R contains an alkylene group having 18 or less carbon atoms; 13a The additive according to [8], wherein the alkyl group has 18 or less carbon atoms.

[0029]

[10] The monovalent sulfur-containing group represented by formula (i-2) is R 11a and p R 12a and R contains an alkylene group having 18 or less carbon atoms; 13a Contains an alkyl group having 18 or less carbon atoms The additive according to [8], which has a melting point of 91°C or lower under normal pressure.

[0030]

[11] The monovalent sulfur-containing group represented by formula (i-2) is R 11a and p R 12a and R contains an alkylene group having 12 or less carbon atoms; 13a The additive according to [8], wherein the alkyl group has 12 or less carbon atoms and has a melting point of 91° C. or less under normal pressure.

[0031]

[12] The monovalent sulfur-containing group represented by formula (i-2) is R 11a and p R12a and R contains an alkylene group having 10 or less carbon atoms; 13a The additive according to [8], wherein the additive has an alkyl group having 10 or less carbon atoms and a melting point of 91°C or less under normal pressure.

[0032]

[13] The monovalent sulfur-containing group represented by formula (i-2) is R 11a and p R 12a and R contains an alkylene group having 10 or less carbon atoms; 13a The additive according to [8], wherein the additive has a melting point of less than 70°C under normal pressure.

[0033]

[14] The monovalent sulfur-containing group represented by formula (i-2) is R 11a and p R 12a and R contains an alkylene group having 8 or less carbon atoms. 13a The additive according to [8], wherein the alkyl group has 8 or less carbon atoms and has a melting point of less than 70°C under normal pressure.

[0034]

[15] The monovalent sulfur-containing group represented by formula (i-2) is R 11a and p R 12a and R contains an alkylene group having 8 or less carbon atoms. 13a The additive according to [8], wherein the additive has a melting point of 35° C. or lower under normal pressure.

[0035]

[16] R represents a monovalent sulfur-containing group represented by formula (i-2). 6a ~R 9a The additive according to [1] or [2], wherein the additive has the following structure at any one of the positions:

[0036]

[17] The monovalent sulfur-containing group represented by formula (i-2) is a group in which n is 0 and p R 12a contains an alkylene group having 18 or less carbon atoms, and R 13a The additive according to

[16] , wherein the alkyl group has 18 or less carbon atoms.

[0037]

[18] The monovalent sulfur-containing group represented by formula (i-2) is a group in which n is 0 and p R 12a contains an alkylene group having 8 or less carbon atoms, and R13a The additive according to

[16] , wherein the additive has an alkyl group having 8 or less carbon atoms and a melting point of less than 70°C under normal pressure.

[0038]

[19] The monovalent sulfur-containing group represented by formula (i-2) is a group in which n and p are 0, and R 13a The additive according to

[16] , wherein the alkyl group has 18 or less carbon atoms.

[0039]

[20] The monovalent sulfur-containing group represented by formula (i-2) is a group in which n and p are 0, and R 13a The additive according to

[16] , wherein the additive has an alkyl group having 18 or less carbon atoms and a melting point of 91° C. or less under normal pressure.

[0040]

[21] The monovalent sulfur-containing group represented by formula (i-2) is a group in which n and p are 0, and R 13a The additive according to

[16] , wherein the alkyl group has 12 or less carbon atoms and has a melting point of 91° C. or less under normal pressure.

[0041]

[22] The monovalent sulfur-containing group represented by formula (i-2) is a group in which n and p are 0, and R 13a The additive according to

[16] , wherein the additive has an alkyl group having 10 or less carbon atoms and a melting point of 91° C. or less under normal pressure.

[0042]

[23] The monovalent sulfur-containing group represented by formula (i-2) is a group in which n and p are 0, and R 13a The additive according to

[16] , wherein the additive has a melting point of 91° C. or lower under normal pressure.

[0043]

[24] The monovalent sulfur-containing group represented by formula (i-2) is a group in which n and p are 0, and R 13a The additive according to

[16] , wherein the additive has a melting point of less than 70° C. under normal pressure.

[0044]

[25] The monovalent sulfur-containing group represented by formula (i-2) is a group in which n and p are 0, and R 13a and has a melting point of 35° C. or lower under normal pressure.

[0045]

[26] R 1a ~R 5a 26. The additive according to claim 17, wherein the substituents are selected from a methyl group, a t-butyl group, and a hydroxy group, and the number of t-butyl groups is not more than one.

[0046]

[27] The additive according to any one of

[16] to

[26] , wherein the light absorption peak in a 100 μM chloroform solution is at 350 to 390 nm, and the absolute value of the slope of the line connecting this absorption peak and the peak end of the absorption spectrum on the long wavelength side is 0.025 or more.

[0047]

[28] R represents a monovalent sulfur-containing group represented by formula (i-2). 7a or R 8a The additive according to

[27] , wherein the additive has the structure:

[0048]

[29] R 1a ~R 5a The additive according to

[16] , wherein the substituents are selected from a methyl group, a t-butyl group, and a hydroxy group, and the number of t-butyl groups is one or less.

[0049]

[30] R 1a ~R 5a is selected from a methyl group, a t-butyl group, and a hydroxy group, and the number of t-butyl groups is one or less.

[0050]

[31] An additive for imparting ultraviolet absorbing ability and / or a high refractive index to a matrix, which is represented by the following formula (II):

[0051] [ka]

[0052] (In the formula, R 1b ~R 10b each independently represents the following formula (ii-1) or formula (ii-2):

[0053] [ka]

[0054] (In formula (ii-1), R 11b represents a divalent hydrocarbon group having 1 to 12 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, and q represents an integer of 0 or 1. In formula (ii-2), R 12b represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom; R 13b When s is 2 or more, each independently represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, and R 14b R represents a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, which is a monovalent hydrocarbon group having 1 to 20 carbon atoms, in which a hydrogen atom may be substituted, the base end may be interrupted, or the carbon-carbon bond may be interrupted. 12b and s R 13b and R 14b has a total carbon number of 25 or less. r represents an integer of 0 or 1, and s represents an integer of 0 to 3. R represents a monovalent sulfur-containing group represented by the formula (I), a hydrogen atom, a monovalent hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a monovalent group selected from a halogen atom. 1b ~R 10b At least one of the groups is a monovalent sulfur-containing group represented by formula (ii-1) or formula (ii-2).

[32] The additive according to

[31] , wherein the matrix is ​​a transparent resin.

[0055]

[33] The monovalent sulfur-containing group is represented by formula (ii-1), and the monovalent sulfur-containing group represented by formula (ii-1) is a group in which q is 0 or q is 1 and R 11b The additive according to

[31] or

[32] , wherein the alkylene group has 10 or less carbon atoms.

[0056]

[34] The monovalent sulfur-containing group is represented by formula (ii-1), and the monovalent sulfur-containing group represented by formula (ii-1) is a group in which q is 0 or q is 1 and R 11b and has a melting point of 91° C. or lower under normal pressure.

[0057]

[35] The monovalent sulfur-containing group is represented by formula (ii-1), and the monovalent sulfur-containing group represented by formula (ii-1) is a group in which q is 0 or q is 1 and R 11b contains an alkylene group having 8 or less carbon atoms and has a melting point of less than 70°C under normal pressure.

[0058]

[36] The monovalent sulfur-containing group is represented by formula (ii-1), and the monovalent sulfur-containing group represented by formula (ii-1) is a group in which q is 0 or q is 1 and R 11b contains an alkylene group having 8 or less carbon atoms, and has a melting point of 35° C. or lower under normal pressure.

[0059]

[37] The monovalent sulfur-containing group is represented by formula (ii-1), and the monovalent sulfur-containing group represented by formula (ii-1) is a group in which q is 0 or q is 1 and R 11b is an oxyalkylene group having 10 or less carbon atoms and an ether bond at a base end.

[0060]

[38] The monovalent sulfur-containing group is represented by formula (ii-2), and the monovalent sulfur-containing group represented by formula (ii-2) is R 12b and s R 13band R contains an alkylene group having 18 or less carbon atoms; 14b The additive according to

[31] or

[32] , wherein the alkyl group has 18 or less carbon atoms.

[0061]

[39] The monovalent sulfur-containing group is represented by formula (ii-2), and the monovalent sulfur-containing group represented by formula (ii-2) is R 12b and s R 13b and R contains an alkylene group having 18 or less carbon atoms; 14b The additive according to

[31] or

[32] , wherein the additive has an alkyl group having 18 or less carbon atoms and a melting point of 91° C. or less under normal pressure.

[0062]

[40] The monovalent sulfur-containing group is represented by formula (ii-2), and the monovalent sulfur-containing group represented by formula (ii-2) is R 12b and s R 13b and R contains an alkylene group having 12 or less carbon atoms; 14b The additive according to

[31] or

[32] , wherein the additive has an alkyl group having 12 or less carbon atoms and a melting point of 91° C. or less under normal pressure.

[0063]

[41] The monovalent sulfur-containing group is represented by formula (ii-2), and the monovalent sulfur-containing group represented by formula (ii-2) is R 12b and s R 13b and R contains an alkylene group having 10 or less carbon atoms; 14b The additive according to

[31] or

[32] , wherein the additive has an alkyl group having 10 or less carbon atoms and a melting point of 91° C. or less under normal pressure.

[0064]

[42] The monovalent sulfur-containing group is represented by formula (ii-2), and the monovalent sulfur-containing group represented by formula (ii-2) is R 12b and s R 13b and R contains an alkylene group having 10 or less carbon atoms; 14b The additive according to

[31] or

[32] , wherein the additive has an alkyl group having 10 or less carbon atoms and a melting point of less than 70° C. under normal pressure.

[0065]

[43] The monovalent sulfur-containing group is represented by formula (ii-2), and the monovalent sulfur-containing group represented by formula (ii-2) is R 12b and s R 13b and R contains an alkylene group having 8 or less carbon atoms. 14b The additive according to

[31] or

[32] , wherein the additive has an alkyl group having 8 or less carbon atoms and a melting point of less than 70°C under normal pressure.

[0066]

[44] The monovalent sulfur-containing group is represented by formula (ii-2), and the monovalent sulfur-containing group represented by formula (ii-2) is R 12b and s R 13b and R contains an alkylene group having 8 or less carbon atoms. 14b and has a melting point of 35° C. or lower under normal pressure.

[0067]

[45] An additive for imparting ultraviolet absorbing ability and / or a high refractive index to a matrix, represented by the following formula (III):

[0068] [ka]

[0069] (In the formula, R 1c ~R 10c each independently represents the following formula (iii-1) or formula (iii-2):

[0070] [ka]

[0071] (In formula (iii-1), R 11c represents a divalent hydrocarbon group having 1 to 12 carbon atoms in which a hydrogen atom is substituted, at least one of both ends is interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, and t represents an integer of 0 or 1. In formula (iii-2), R12c represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom; R 13c When v is 2 or more, each independently represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom is substituted, at least one of both ends is interrupted, or the carbon-carbon bond may be interrupted by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, and R 14c R represents a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, which is a monovalent hydrocarbon group having 1 to 20 carbon atoms, in which a hydrogen atom may be substituted, the base end may be interrupted, or the carbon-carbon bond may be interrupted. 12c and v R 13c and R 14c has a total carbon number of 25 or less. u represents an integer of 0 or 1, and v represents an integer of 0 to 3. R represents a monovalent sulfur-containing group represented by the formula (I), a hydrogen atom, a monovalent hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a monovalent group selected from a halogen atom. 1c ~R 10c At least one of the groups is a monovalent sulfur-containing group represented by formula (iii-1) or formula (iii-2).

[46] The additive according to

[45] , wherein the matrix is ​​a transparent resin.

[0072]

[47] The monovalent sulfur-containing group is represented by formula (iii-1), and the monovalent sulfur-containing group represented by formula (iii-1) is a monovalent sulfur-containing group represented by formula (iii-1) in which t is 0 or t is 1 and R 11c 45. The additive according to claim 43 or 44, wherein comprises an alkylene group having 10 or less carbon atoms.

[0073]

[48] ​​The monovalent sulfur-containing group is represented by formula (iii-1), and the monovalent sulfur-containing group represented by formula (iii-1) is a group in which t is 0 or t is 1 and R 11c and has a melting point of 91° C. or lower under normal pressure.

[0074]

[49] The monovalent sulfur-containing group is represented by formula (iii-1), and the monovalent sulfur-containing group represented by formula (iii-1) is a monovalent sulfur-containing group represented by formula (iii-1), in which t is 0 or t is 1 and R 11c The additive according to

[45] or

[46] , wherein the additive has an alkylene group having 8 or less carbon atoms and a melting point of less than 70°C under normal pressure.

[0075]

[50] The monovalent sulfur-containing group is represented by formula (iii-1), and the monovalent sulfur-containing group represented by formula (iii-1) is a monovalent sulfur-containing group represented by formula (iii-1), in which t is 0 or t is 1 and R 11c and has a melting point of 35° C. or lower under normal pressure.

[0076]

[51] The monovalent sulfur-containing group is represented by formula (iii-1), and the monovalent sulfur-containing group represented by formula (iii-1) is a group in which t is 0 or t is 1 and R 11c is an oxyalkylene group having 10 or less carbon atoms and an ether bond at a base end.

[0077]

[52] The monovalent sulfur-containing group is represented by formula (iii-2), and the monovalent sulfur-containing group represented by formula (iii-2) is R 12c and v R 13c and R contains an alkylene group having 18 or less carbon atoms; 14c The additive according to

[45] or

[46] , wherein the alkyl group has 18 or less carbon atoms.

[0078]

[53] The monovalent sulfur-containing group is represented by formula (iii-2), and the monovalent sulfur-containing group represented by formula (iii-2) is R 12c and v R13c and R contains an alkylene group having 18 or less carbon atoms; 14c The additive according to

[45] or

[46] , wherein the additive has an alkyl group having 18 or less carbon atoms and a melting point of 91° C. or less under normal pressure.

[0079]

[54] The monovalent sulfur-containing group is represented by formula (iii-2), and the monovalent sulfur-containing group represented by formula (iii-2) is R 12c and v R 13c and R contains an alkylene group having 12 or less carbon atoms; 14c The additive according to

[45] or

[46] , wherein the additive has a melting point of 91° C. or lower under normal pressure.

[0080]

[55] The monovalent sulfur-containing group is represented by formula (iii-2), and the monovalent sulfur-containing group represented by formula (iii-2) is R 12c and v R 13c and R contains an alkylene group having 10 or less carbon atoms; 14c The additive according to

[45] or

[46] , wherein the additive has an alkyl group having 10 or less carbon atoms and a melting point of 91° C. or less under normal pressure.

[0081]

[56] The monovalent sulfur-containing group is represented by formula (iii-2), and the monovalent sulfur-containing group represented by formula (iii-2) is R 12c and v R 13c and R contains an alkylene group having 10 or less carbon atoms; 14c The additive according to

[45] or

[46] , wherein the additive has an alkyl group having 10 or less carbon atoms and a melting point of less than 70°C under normal pressure.

[0082]

[57] The monovalent sulfur-containing group is represented by formula (iii-2), and the monovalent sulfur-containing group represented by formula (iii-2) is R 12c and v R 13c and R contains an alkylene group having 8 or less carbon atoms. 14c The additive according to

[45] or

[46] , wherein the additive has an alkyl group having 8 or less carbon atoms and a melting point of less than 70°C under normal pressure.

[0083]

[58] The monovalent sulfur-containing group is represented by formula (iii-2), and the monovalent sulfur-containing group represented by formula (iii-2) is R 12c and v R 13c and R contains an alkylene group having 8 or less carbon atoms. 14c and has a melting point of 35° C. or lower under normal pressure.

[0084]

[59] An additive for imparting ultraviolet absorbing ability and / or a high refractive index to a matrix, represented by the following formula (IV):

[0085] [ka]

[0086] (In the formula, R 1d ~R 15d each independently represents the following formula (iv-1) or formula (iv-2):

[0087] [ka]

[0088] (In formula (iv-1), R 16d is a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, and represents a divalent hydrocarbon group having 1 to 12 carbon atoms in which a hydrogen atom may be substituted, at least one of the ends may be interrupted, or the carbon-carbon bond may be interrupted, and w represents an integer of 0 or 1. In formula (iv-2), R 17d represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom; R 18dWhen y is 2 or more, each independently represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom; R 19d R represents a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, which is a monovalent hydrocarbon group having 1 to 20 carbon atoms, in which a hydrogen atom may be substituted, the base end may be interrupted, or the carbon-carbon bond may be interrupted. 17d and y R 18d and R 19d has a total carbon number of 25 or less. x represents an integer of 0 or 1, and y represents an integer of 0 to 3. R represents a monovalent sulfur-containing group represented by the formula (I), a hydrogen atom, a monovalent hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a monovalent group selected from a halogen atom. 1d ~R 15d At least one of the groups is a monovalent sulfur-containing group represented by formula (iv-1) or formula (iv-2).

[60] The additive according to

[59] , wherein the matrix is ​​a transparent resin.

[0089]

[61] The monovalent sulfur-containing group is represented by formula (iv-1) or formula (iv-2). In the monovalent sulfur-containing group represented by formula (iv-1), w is 0 or w is 1 and R 16d contains an alkylene group having 8 or less carbon atoms, and the monovalent sulfur-containing group represented by formula (iv-2) is R 17d and y R 18d and R contains an alkylene group having 8 or less carbon atoms. 19d The additive according to

[59] or

[60] , wherein the alkyl group has 8 or less carbon atoms.

[0090]

[62] An additive for imparting ultraviolet absorbing ability and / or a high refractive index to a matrix, represented by the following formula (V):

[0091] [ka]

[0092] (In the formula, R 1e ~R 9e R each independently represents a monovalent group selected from an alkyl group having 10 to 24 carbon atoms, the linear chain of which may be substituted with two or less alkyl groups each having 1 or 2 carbon atoms, a hydrogen atom, a monovalent hydrocarbon group having 1 to 4 carbon atoms, an aromatic group, an unsaturated group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom. 1e ~R 9e At least one of the groups is the alkyl group having 10 to 24 carbon atoms.)

[63] The additive according to

[62] , wherein the matrix is ​​a transparent resin.

[0093]

[64] The additive of the present invention is the additive according to any one of [1] to

[64] , wherein R 1a ~R 13a , R 1b ~R 14b , R 1c ~R 14c , R 1d ~R 19d A reactive functional group is bonded to at least one group selected from the group consisting of:

[0094]

[65] The resin member of the present invention contains the additive according to any one of [1] to

[15] and

[31] to

[64] in a matrix resin.

[0095]

[66] The transparent resin workpiece of the present invention contains the additive according to any one of [1] to

[15] and

[31] to

[64] in a matrix resin.

[0096]

[67] The resin workpiece of the present invention contains the additive according to any one of

[16] to

[30] in a matrix resin.

[0097]

[68] The transparent resin workpiece of the present invention contains the additive according to any one of

[16] to

[30] in a matrix resin.

[0098]

[69] The resin member of the present invention is a resin member according to any one of

[65] to

[68] , which is one layer of a member having a laminated multilayer structure, a film, a sheet, a plate-shaped member, or an optical resin. Effect of the Invention

[0099] The additive of the present invention has good compatibility with the matrix resin, is excellent in heat resistance, and can maintain high transparency even when added at low to high concentrations. Therefore, the additive can fully exhibit the performance of imparting ultraviolet absorbing ability and high refractive index by adding at a high concentration while maintaining transparency.

[0100] Furthermore, the additive of the present invention can provide both the ultraviolet absorbing ability and the function of providing a high refractive index with a single additive.

[0101] Due to the heat resistance of the additive and its compatibility with the resin, the resin workpiece containing the additive of the present invention has transparency even under a wide range of additive concentration conditions from low to high, and is endowed with a high refractive index and / or ultraviolet absorbing ability. In particular, under high concentration conditions, the transparency is maintained and a higher refractive index and / or ultraviolet absorbing ability can be imparted. In addition, the laminated multi-layer structure is simplified, making it possible to reduce the manufacturing process and costs. Furthermore, it can be applied to high resin molding processing temperatures. [Brief description of the drawings]

[0102] [Figure 1] 1 shows ultraviolet-visible absorption spectra (UV chart) of Examples 36 to 40 (benzotriazole type). [Diagram 2] 1 shows ultraviolet-visible absorption spectra (UV charts) of Examples 41 to 44 and Comparative Example 9 (benzotriazole-based). [Diagram 3] 1 is an ultraviolet-visible absorption spectrum (UV chart) of Examples 45 to 49 (benzotriazole type). [Figure 4]1 is an ultraviolet-visible absorption spectrum (UV chart) of Examples 50 to 54 (benzotriazole type). [Diagram 5] 1 shows ultraviolet-visible absorption spectra (UV charts) of Examples 55 to 60 and Comparative Example 10 (benzotriazole-based). [Figure 6] 1 shows ultraviolet-visible absorption spectra (UV charts) of Examples 61 to 64 and Comparative Example 11 (benzophenone-based). [Figure 7] 1 shows ultraviolet-visible absorption spectra (UV charts) of Examples 65 and 66 and Comparative Example 12 (salicylate type). [Figure 8] 1 shows ultraviolet-visible absorption spectra (UV charts) of Examples 67 to 70 and Comparative Example 13 (triazine-based). [Figure 9] The absorption peak of compound 21 was measured at concentrations of 10, 25, and 50 μM, and the absolute value of the slope on the long wavelength side of the absorption peak in the wavelength region of 350 to 390 nm was plotted against the concentration of the ultraviolet absorber. [Figure 10] 1 shows transmission spectra of plastic lenses of Example 71 and Comparative Example 14. [Figure 11] 1 shows transmission spectra of plastic lenses of Example 72 and Comparative Example 15. [Figure 12] 1 shows transmission spectra of plastic lenses of Example 73 and Comparative Example 16. [Figure 13] 1 shows transmission spectra of plastic lenses of Example 74 and Comparative Example 17. [Figure 14] 1 shows transmission spectra of plastic lenses of Example 75 and Comparative Example 18. [Figure 15] 1 shows transmission spectra of plastic lenses of Example 76 and Comparative Example 14. [Figure 16] 1 shows transmission spectra of plastic lenses of Example 77 and Comparative Example 14. [Figure 17] Photographs of the films of Examples 10 and 13. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0103] The present invention will be described in detail below.

[0104] The additives represented by the above formulas (I) to (IV) are characterized by the introduction of a sulfur-containing group into the ultraviolet absorbing skeleton of a benzotriazole, benzophenone, salicylate, or triazine. The introduction of this sulfur-containing group improves compatibility with the matrix resin, and high transparency can be maintained even when added at a high concentration. In addition, the weight loss temperature increases and heat resistance is improved. Furthermore, the ultraviolet absorbing skeleton exhibits ultraviolet absorbing ability, and the sulfur-containing group exhibits performance as a high refractive index imparting agent. [Substituents, etc.] In the present invention, the "monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom" includes a group capable of imparting a high refractive index, a group capable of adjusting heat resistance and compatibility with a resin, a group reactive with a resin and / or a monomer of a resin, and the like, and includes, for example, the following: (aromatic group) The aromatic group contains an aromatic ring such as a benzene ring, a naphthalene ring, or an anthracene ring, and has a carbon number of preferably 6 to 18, more preferably 6 to 14. Examples of the monovalent or divalent aromatic group include a phenyl group, a 2-methylphenyl group, a 3-methylphenyl group, a 4-methylphenyl group, a 2,4-dimethylphenyl group, a 2,5-dimethylphenyl group, a 3,4-dimethylphenyl group, a 3,5-dimethylphenyl group, a 2,4,5-trimethylphenyl group, a 2,4,6-trimethylphenyl group, a 4-biphenyl group, a 1-naphthyl group, a 2-methoxyphenyl group, a 3-methoxyphenyl group, a 4-methoxyphenyl group, a 2-ethoxyphenyl group, a 3-ethoxyphenyl group, a 4-ethoxyphenyl group, a 2-chlorophenyl group, a 2-fluorophenyl group, a 4-fluorophenyl group, a 2-trifluoromethylphenyl group, a 4-trifluoromethylphenyl group, a 1-naphthyl group, and a 2-naphthyl group. (unsaturated group) The unsaturated group contains a carbon-carbon or carbon-heteroatom unsaturated bond such as a carbon-carbon double bond, a carbon-carbon triple bond, a carbon-oxygen double bond (carbonyl group, aldehyde group, carboxyl group, etc.), a carbon-nitrogen double bond (isocyanate group, etc.), a carbon-nitrogen triple bond (cyano group, cyanato group, etc.), and has a carbon number of preferably 1 to 10, more preferably 1 to 8. Examples of the monovalent or divalent unsaturated group include an acryloyl group, a methacryloyl group, a maleic acid monoester group, a styryl group, an allyl group, a vinyl group, an amide group, a carbamoyl group, a cyano group, an isocyanate group, etc. (sulfur-containing group) The sulfur-containing group includes a thiol group, a sulfide group, a disulfide group, a sulfonyl group, a sulfo group, a thiocarbonyl group, a thiocarbamoyl group, or a thiourea group, and the number of carbon atoms is preferably 0 to 10. Examples of the monovalent or divalent sulfur-containing group include a thiomethoxy group, a thioethoxy group, a thio-n-propoxy group, a thioisopropoxy group, a thio-n-butoxy group, a thio-t-butoxy group, a thiophenoxy group, a p-methylthiophenoxy group, a p-methoxythiophenoxy group, a thiophene group, a thiazole group, a thiol group, a sulfo group, a sulfide group, a disulfide group, a sulfonyl group, a thiocarbonyl group, and a thiourea group. (oxygen-containing group) When the oxygen-containing group contains an aromatic ring group or an alicyclic group, the carbon number is preferably 6 to 12, and when the oxygen-containing group does not contain an aromatic ring group or an alicyclic group, the carbon number is preferably 0 to 6. Examples of the monovalent or divalent oxygen-containing group include a hydroxy group, a methoxy group, an ethoxy group, a propoxy group, a butoxy group, a phenoxy group, a methylphenoxy group, a dimethylphenoxy group, a naphthoxy group, a phenylmethoxy group, a phenylethoxy group, an acetoxy group, an acetyl group, an aldehyde group, a carboxyl group, a carbamoyl group, a urea group, an ether group, a carbonyl group, an ester group, an oxazole group, and a morpholine group. (phosphorus-containing group) The phosphorus-containing group contains a phosphine group, a phosphite group, a phosphonic acid group, a phosphinic acid group, a phosphoric acid group, or a phosphoric acid ester group, and when it contains an aromatic ring group or an alicyclic group, it preferably has 6 to 22 carbon atoms, and when it does not contain an aromatic ring group or an alicyclic group, it preferably has 0 to 6 carbon atoms. Examples of the monovalent or divalent phosphorus-containing group include a trimethylphosphine group, a tributylphosphine group, a tricyclohexylphosphine group, a triphenylphosphine group, a tritolylphosphine group, a methylphosphine group, an ethylphosphite group, a phenylphosphite group, a phosphonic acid group, a phosphinic acid group, a phosphoric acid group, and a phosphoric acid ester group. (alicyclic group) The number of carbon atoms in the alicyclic group is preferably 3 to 10, more preferably 3 to 8. Examples of the monovalent or divalent alicyclic group include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, and a cyclooctyl group. (Halogen atom) Examples of the halogen atom include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.

[0105] The additive represented by the formula (V) is characterized by the introduction of a long-chain alkyl group into a benzotriazole-based UV-absorbing skeleton. The introduction of this long-chain alkyl group makes the additive liquid, and improves its compatibility with the matrix resin, so that it can maintain high transparency even when added at a high concentration. As a result, a resin part having high transparency and high UV-absorbing ability can be obtained. 1. Additive represented by formula (I) The additive represented by the above formula (I) contains a monovalent sulfur-containing group represented by the above formula (i-1) or (i-2) in a benzotriazole-based skeleton.

[0106] In formula (i-1), R 10arepresents a divalent hydrocarbon group having 1 to 12 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0107] R 10a Examples of the divalent hydrocarbon group include linear or branched alkylene groups, alkenylene groups, alkynylene groups, etc. Specific examples include methylene group, ethane-1,2-diyl group, propane-1,3-diyl group, 1-methylethane-1,2-diyl group, butane-1,4-diyl group, butane-1,3-diyl group, 2-methylpropane-1,3-diyl group, pentane-1,5-diyl group, pentane-1,4-diyl group, hexane-1,6-diyl group, heptane-1,7-diyl group, octane-1,8-diyl group, nonane-1,9-diyl group, decane-1,10-diyl group, undecane-1,11-diyl group, dodecane-1,12-diyl group, etc.

[0108] When a divalent hydrocarbon group has a hydrogen atom substituted with the monovalent or divalent group, at least one of its ends interrupted, or a carbon-carbon bond interrupted, the number of the monovalent or divalent groups is preferably 2 or less, more preferably 1 or less.

[0109] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0110] In formula (i-1), m represents an integer of 0 or 1.

[0111] In formula (i-2), R 11arepresents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0112] R 11a Examples of the divalent hydrocarbon group include linear or branched alkylene groups, linear or branched alkenylene groups, linear or branched alkynylene groups, etc. Specific examples include methylene groups, ethane-1,2-diyl groups, propane-1,3-diyl groups, 1-methylethane-1,2-diyl groups, butane-1,4-diyl groups, butane-1,3-diyl groups, 2-methylpropane-1,3-diyl groups, pentane-1,5-diyl groups, pentane-1,4-diyl groups, hexane-1,6-diyl groups, heptane-1,7-diyl groups, octane-1,8-diyl groups, nonane-1,9-diyl groups, and the like. -diyl group, decane-1,10-diyl group, undecane-1,11-diyl group, dodecane-1,12-diyl group, tridecane-1,13-yl group, tetradecane-1,14-yl group, pentadecane-1,15-yl group, hexadecane-1,16-yl group, heptadecane-1,17-yl group, octadecane-1,18-yl group, nonadecane-1,19-yl group, eicosan-1,20-yl group, etc. Among these, alkylene groups are preferred, and linear alkylene groups are more preferred.

[0113] R 11a In the case where a hydrogen atom is substituted, at least one of both ends is interrupted, or the carbon-carbon bond is interrupted by the monovalent or divalent group, the number of monovalent or divalent groups is preferably 2 or less, and more preferably 1 or less.

[0114] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0115] In formula (i-2), R12a When p is 2 or more, each independently represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0116] R 12a As the divalent hydrocarbon group, R 11a Among these, alkylene groups are preferred, and linear alkylene groups are more preferred.

[0117] R 12a In the case where a hydrogen atom of the divalent hydrocarbon group is substituted with the monovalent or divalent group, or at least one of the terminals is interrupted, or the carbon-carbon bond is interrupted, the number of the monovalent or divalent groups is preferably 2 or less, and more preferably 1 or less.

[0118] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0119] In formula (i-2), R 13a represents a hydrogen atom or -(R 14a ) l -R 15a A group represented by R 14a represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, the terminal may be interrupted, or the carbon-carbon bond may be interrupted by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom; R 15a represents a hydrogen atom or a substituent containing any one skeleton selected from benzotriazole, benzophenone, benzoic acid ester, and triazine. 1 represents an integer of 0 or 1.

[0120] R14a As the divalent hydrocarbon group, R 10a Among these, alkylene groups are preferred, and linear alkylene groups are more preferred.

[0121] R 14a When a divalent hydrocarbon group has a hydrogen atom substituted, a base end interrupted, or a carbon-carbon bond interrupted by said monovalent or divalent group, the number of said monovalent or divalent groups is preferably 2 or less, and more preferably 1 or less.

[0122] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0123] R 15a is a substituent containing any one skeleton selected from benzotriazole, benzophenone, benzoic acid ester, and triazine, examples of the substituent containing benzotriazole include a group represented by the following formula (A), examples of the substituent containing benzophenone include a group represented by the following formula (B), examples of the substituent containing benzoic acid ester include a group represented by the following formula (C), and examples of the substituent containing triazine include a group represented by the following formula (D).

[0124] [ka]

[0125] In formula (A), R 16a ~R 24a Any one of the formula (i-2) is R 14a or a monovalent bond to a terminal sulfur atom, and other R 16a ~R 24a each independently represents a monovalent group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0126] [ka]

[0127] In formula (B), R 15b ~R 24b Any one of the formula (i-2) is R 14a or a monovalent bond to a terminal sulfur atom, and other R 15b ~R 24b each independently represents a monovalent group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0128] [ka]

[0129] In formula (C), R 15c ~R 24c Any one of the formula (i-2) is R 14a or a monovalent bond to a terminal sulfur atom, and other R 15c ~R 24c each independently represents a monovalent group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0130] [ka]

[0131] In formula (D), R 20d ~R 22d indicates either [A] or [B] below. [A]R 20d ~R 22d At least one of the R 14a or a monovalent bond to a terminal sulfur atom, and other R 20d ~R22d each independently represents a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, a halogen atom, or a group represented by the following formula (d):

[0132] [ka]

[0133] (In the formula, R 23d ~R 27d each independently represents a monovalent group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.) In other words, 1 to 3 groups represented by formula (I) may be bonded to the triazine ring. [I]R 20d ~R 22d At least one of the groups represented by the following formula (d'):

[0134] [ka]

[0135] (R 28d ~R 32d At least one of the R 14a or a monovalent bond to a terminal sulfur atom, and other R 28d ~R 32d each independently represents a monovalent group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom; 20d ~R 22d each independently represents a monovalent group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom. That is, the benzene ring represented by the above formula (d') may have 1 to 5 groups represented by formula (I) bonded thereto.

[0136] In formulas (A) to (D) and (d), R 16a ~R 24a , R 15b ~R 24b , R 15c ~R 24c , R 20d ~R 27d is a monovalent hydrocarbon group, examples of the monovalent hydrocarbon group include linear or branched alkyl groups, linear or branched alkenyl groups, linear or branched alkynyl groups, etc. Specific examples include methyl group, ethane-1-yl group, propane-1-yl group, 1-methylethane-1-yl group, butane-1-yl group, butane-2-yl group, 2-methylpropane-1-yl group, 2-methylpropane-2-yl group, pentan-1-yl group, pentan-2-yl group, hexane-1-yl group, heptan-1-yl group, octan-1-yl group, nonane-1-yl group, decan-1-yl group, etc.

[0137] R 16a ~R 24a , R 15b ~R 24b , R 15c ~R 24c , R 20d ~R 27d When is a monovalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, specific examples thereof include those exemplified in the above column of [Substituents, etc.]. In formula (i-2), n represents an integer of 0 or 1; p represents an integer of 0 to 3, preferably 0 or 1.

[0138] In formula (i-2), R 11a and p R 12a and R 13a The total number of carbon atoms is 25 or less.

[0139] In formula (I), R 1a ~R 9ais a group other than the monovalent sulfur-containing group represented by formula (i-1) or formula (i-2), it represents a monovalent group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0140] R 1a ~R 9a When is a monovalent hydrocarbon group, examples of the monovalent hydrocarbon group include linear or branched alkyl groups, linear or branched alkenyl groups, and linear or branched alkynyl groups. Specific examples include methyl, ethane-1-yl, propane-1-yl, 1-methylethane-1-yl, butane-1-yl, butane-2-yl, 2-methylpropane-1-yl, 2-methylpropane-2-yl, pentan-1-yl, pentan-2-yl, hexane-1-yl, heptan-1-yl, octan-1-yl, nonane-1-yl, and decan-1-yl groups. Among these, linear or branched alkyl groups having 1 to 8 carbon atoms are preferred.

[0141] R 1a ~R 9a When is a monovalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, specific examples thereof include those exemplified in the above column of [Substituents, etc.].

[0142] In formula (I), R 1a ~R 9a Among them, at least one of them is a monovalent sulfur-containing group represented by formula (i-1) or formula (i-2). Among them, taking into consideration the ease of actual synthesis, cost, heat resistance, or compatibility with the matrix resin to suppress clouding of the resin member to which the additive of the present invention is added, and the ability to express high ultraviolet absorption ability or impart a high refractive index when added at a high concentration, R 1a ~R 9a Among these, it is preferred that one or two of them are monovalent sulfur-containing groups represented by formula (i-1) or formula (i-2).

[0143] The position of the monovalent sulfur-containing group represented by formula (i-1) or formula (i-2) in formula (I) is not particularly limited, but R 1a , R 3a , R 5a , R 7a or R 8a Examples include:

[0144] The additive of formula (I) incorporating (i-1) as a monovalent sulfur-containing group is capable of exhibiting heat resistance, high ultraviolet absorbing ability when added at low to high concentrations, or imparting a high refractive index. In consideration of this, the monovalent sulfur-containing group represented by formula (i-1) is preferably selected from the group consisting of m being 0, m being 1, and R 10a It is preferred that the alkylene group contains up to 10 carbon atoms.

[0145] In addition, the melting point of these additives tends to decrease when the number of carbon atoms is adjusted by introducing a sulfur-containing group. When the melting point is decreased, the compatibility with the matrix resin becomes particularly good. From this point of view, the monovalent sulfur-containing group represented by formula (i-1) is such that m is 0 or m is 1 and R 10a It is preferable that the compound contains an alkylene group having 9 or less carbon atoms and has a melting point of 91° C. or less under normal pressure (for example, standard atmospheric pressure of 101,325 Pa).

[0146] In another preferred embodiment, the monovalent sulfur-containing group represented by formula (i-1) is such that m is 0 or m is 1 and R 10a contains an alkylene group having 8 or less carbon atoms, and has a melting point of less than 70° C. under normal pressure. Alternatively, the monovalent sulfur-containing group represented by formula (i-1) is such that m is 0 or m is 1 and R 10a contains an alkylene group having 8 or less carbon atoms and has a melting point of 35° C. or less under normal pressure. In other words, when the carbon number is 8 or less and the melting point is less than 70° C., high transparency can be obtained in a thick film thickness even if added at a high concentration, and further, when it is liquid at room temperature (5 to 35° C.), high transparency can be realized in an even thicker film thickness even if added at a high concentration.

[0147] The additive of formula (I) incorporating (i-2) as a monovalent sulfur-containing group is capable of exhibiting heat resistance, high ultraviolet absorbing ability when added at low to high concentrations, or imparting a high refractive index. In consideration of this, the monovalent sulfur-containing group represented by formula (i-2) is R 11a and p R 12a and R contains an alkylene group having 18 or less carbon atoms; 13a It is preferred that the alkyl group contains up to 18 carbon atoms.

[0148] In addition, when a sulfur-containing group is introduced into these additives to adjust the number of carbon atoms from a short chain to a medium chain, the melting point tends to decrease. When the melting point decreases, the compatibility with the matrix resin becomes particularly good. In consideration of this point, the monovalent sulfur-containing group represented by formula (i-2) is R 11a and p R 12a and R contains an alkylene group having 18 or less carbon atoms; 13a It is preferable that the copolymer contains an alkyl group having 18 or less carbon atoms and has a melting point of 91° C. or less under normal pressure.

[0149] R represents a monovalent sulfur-containing group represented by formula (i-1) or formula (i-2). 1a ~R 5a In a preferred embodiment, the monovalent sulfur-containing group represented by formula (i-1) is such that m is 0 or m is 1 and R 10a contains an alkylene group having 8 or less carbon atoms, and the monovalent sulfur-containing group represented by formula (i-2) is R 11a and p R 12a and R contains an alkylene group having 8 or less carbon atoms. 13a In a more preferred embodiment, the monovalent sulfur-containing group represented by formula (i-1) is such that m is 0 or m is 1 and R 10a contains an alkylene group having 8 or less carbon atoms, and the monovalent sulfur-containing group represented by formula (i-2) is R 11a and p R 12a and R contains an alkylene group having 8 or less carbon atoms. 13a It contains an alkyl group having 8 or less carbon atoms, and has a melting point of 35°C or less under normal pressure. (An ultraviolet absorber that has excellent heat resistance and provides ultraviolet absorption and a high refractive index while maintaining the transparency of the transparent resin matrix) Preferred embodiments of the ultraviolet absorbing agent for imparting excellent heat resistance, ultraviolet absorbing ability and a high refractive index while maintaining the transparency of the transparent resin matrix include the following. A monovalent sulfur-containing group represented by formula (i-2) is represented by R 6a ~R 9a and the monovalent sulfur-containing group represented by formula (i-2) is represented by the following formula:

[0150] [ka]

[0151] where p R 12a contains an alkylene group having 1 to 18 carbon atoms, and R 13a Contains an alkyl group having 1 to 18 carbon atoms.

[0152] Furthermore, p R 12a contains an alkylene group having 1 to 8 carbon atoms, and R 13a It contains an alkyl group having 1 to 8 carbon atoms and has a melting point of less than 70° C. under normal pressure. ·R 13a Contains an alkyl group having 1 to 18 carbon atoms. ·R 13a It contains an alkyl group having 1 to 18 carbon atoms and has a melting point of 91° C. or lower under normal pressure. ·R 13a It contains an alkyl group having 1 to 12 carbon atoms and has a melting point of 91° C. or lower under normal pressure. ·R 13a It contains an alkyl group having 1 to 10 carbon atoms and has a melting point of 91° C. or lower under normal pressure. ·R 13a It contains an alkyl group having 4 to 10 carbon atoms and has a melting point of 91° C. or lower under normal pressure. ·R 13a It contains an alkyl group having 6 to 10 carbon atoms and has a melting point of less than 70° C. under normal pressure. ·R 13a It contains an alkyl group having 6 to 10 carbon atoms and has a melting point of 35° C. or lower under normal pressure. The substituents are selected from a methyl group, a t-butyl group, and a hydroxy group, and the number of t-butyl groups is not more than one. Among them, the substituents are R 1a , R 2a , R 4a In particular, R 1a The substituents of are hydroxy groups, R 2a The substituent of is t-butyl group, R 4a The substituent of is a methyl group. (An ultraviolet absorber that absorbs light in the long wavelength range and suppresses yellowing of the transparent resin matrix) In a preferred embodiment, the ultraviolet absorber that absorbs light in the long wavelength region and suppresses yellowing of a transparent resin matrix has a monovalent sulfur-containing group represented by formula (i-2) in R 6a ~R 9a and the monovalent sulfur-containing group represented by formula (i-2) is represented by the following formula:

[0153] [ka]

[0154] (In the formula, R 12a , R 13a and p has the same meaning as above. It is expressed as:

[0155] The additive of formula (I) has high solubility in resin monomers, does not precipitate on the surface when processed into a plastic lens, is highly transparent, and has optical properties that allow it to fully absorb light in the wavelength range of 250 to 420 nm. Moreover, it has a high ultraviolet absorption effect (molar absorption coefficient), and can fully absorb light of that wavelength with the addition of a small amount. In a chloroform solution, the slope of the absorption peak at 350 to 390 nm is greater than that of conventional ultraviolet absorbers, so that yellowing of the resin part can be suppressed.

[0156] In order to absorb harmful light in the wavelength range of 400 to 420 nm, which may trigger damage to eye tissue such as age-related macular degeneration, and to suppress absorption of light with wavelengths of around 420 nm or more, which causes yellowing of lenses, and to obtain a resin part with excellent appearance with suppressed yellowing, the light absorption peak in a 100 μM chloroform solution is preferably 350 to 390 nm, more preferably 360 to 380 nm, and particularly preferably 360 to 375 nm. Furthermore, the absorption peaks in these wavelength ranges are the maximum absorption wavelengths (λ max ). Furthermore, in order to suppress the absorption of light with wavelengths longer than about 420 nm, the absorption spectrum on the long wavelength side is preferably sharp (the absolute value of the slope is larger), and the slope of the absorption peak on the long wavelength side (the absolute value of the slope of the line connecting the absorption peak and the peak end of the absorption spectrum on the long wavelength side: see FIG. 3 and the Examples section described later) is preferably 0.025 or more, more preferably 0.030 or more. In addition, in order to efficiently absorb light with a small amount, the molar absorption coefficient of the absorption peak in the range of 350 to 390 nm (maximum molar absorption coefficient: ελ max ) is preferably 17,000 L / (mol cm) or more, more preferably 18,000 L / (mol cm) or more, and particularly preferably 20,000 L / (mol cm) or more. 2. Additive represented by formula (II) The additive represented by the formula (II) above contains a monovalent sulfur-containing group represented by the formula (ii-1) or (ii-2) above in a benzophenone-based skeleton.

[0157] In formula (ii-1), R 11b represents a divalent hydrocarbon group having 1 to 12 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0158] R 11bExamples of the divalent hydrocarbon group include linear or branched alkylene groups, alkenylene groups, alkynylene groups, etc. Specific examples include methylene group, ethane-1,2-diyl group, propane-1,3-diyl group, 1-methylethane-1,2-diyl group, butane-1,4-diyl group, butane-1,3-diyl group, 2-methylpropane-1,3-diyl group, pentane-1,5-diyl group, pentane-1,4-diyl group, hexane-1,6-diyl group, heptane-1,7-diyl group, octane-1,8-diyl group, nonane-1,9-diyl group, decane-1,10-diyl group, undecane-1,11-diyl group, dodecane-1,12-diyl group, etc.

[0159] When a divalent hydrocarbon group has a hydrogen atom substituted with the monovalent or divalent group, at least one of its ends interrupted, or a carbon-carbon bond interrupted, the number of the monovalent or divalent groups is preferably 2 or less, more preferably 1 or less.

[0160] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0161] In formula (ii-1), q represents an integer of 0 or 1.

[0162] In formula (ii-2), R 12b represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0163] R 12bExamples of the divalent hydrocarbon group include linear or branched alkylene groups, linear or branched alkenylene groups, linear or branched alkynylene groups, etc. Specific examples include methylene groups, ethane-1,2-diyl groups, propane-1,3-diyl groups, 1-methylethane-1,2-diyl groups, butane-1,4-diyl groups, butane-1,3-diyl groups, 2-methylpropane-1,3-diyl groups, pentane-1,5-diyl groups, pentane-1,4-diyl groups, hexane-1,6-diyl groups, heptane-1,7-diyl groups, octane-1,8-diyl groups, nonane-1,9-diyl groups, and the like. -diyl group, decane-1,10-diyl group, undecane-1,11-diyl group, dodecane-1,12-diyl group, tridecane-1,13-yl group, tetradecane-1,14-yl group, pentadecane-1,15-yl group, hexadecane-1,16-yl group, heptadecane-1,17-yl group, octadecane-1,18-yl group, nonadecane-1,19-yl group, eicosan-1,20-yl group, etc. Among these, alkylene groups are preferred, and linear alkylene groups are more preferred.

[0164] R 12b In the case where a hydrogen atom of the divalent hydrocarbon group is substituted with the monovalent or divalent group, or at least one of the terminals is interrupted, or the carbon-carbon bond is interrupted, the number of the monovalent or divalent groups is preferably 2 or less, and more preferably 1 or less.

[0165] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0166] In formula (ii-2), R 13b When s is 2 or more, each independently represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0167] R 13b As the divalent hydrocarbon group, R 12b Among these, alkylene groups are preferred, and linear alkylene groups are more preferred.

[0168] R 13b In the case where a hydrogen atom of the divalent hydrocarbon group is substituted with the monovalent or divalent group, or at least one of the terminals is interrupted, or the carbon-carbon bond is interrupted, the number of the monovalent or divalent groups is preferably 2 or less, and more preferably 1 or less.

[0169] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0170] In formula (ii-2), R 14b represents a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, which is a monovalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted.

[0171] R 14bExamples of the monovalent hydrocarbon group include linear or branched alkyl groups, linear or branched alkenyl groups, and linear or branched alkynyl groups. Specifically, for example, methyl group, ethane-1-yl group, propane-1-yl group, 1-methylethane-1-yl group, butane-1-yl group, butane-2-yl group, 2-methylpropane-1-yl group, 2-methylpropane-2-yl group, pentan-1-yl group, pentan-2-yl group, hexane-1-yl group, heptan-1-yl group, octan-1-yl group, nonane-1-yl group, decan-1-yl group, undecane-1-yl group, dodecane-1-yl group, tridecane-1-yl group, tetradecane-1-yl group, pentadecane-1-yl group, hexadecan-1-yl group, heptadecane-1-yl group, octadecane-1-yl group, nonadecan-1-yl group, eicosan-1-yl group, etc. Among these, alkyl groups are preferred, and linear alkyl groups are more preferred.

[0172] R 14b In the case where a hydrogen atom of the monovalent hydrocarbon group is replaced by the monovalent or divalent group, or at least one of the ends is interrupted, or the carbon-carbon bond is interrupted, the number of the monovalent or divalent groups is preferably 2 or less, and more preferably 1 or less.

[0173] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0174] In formula (ii-2), r represents an integer of 0 or 1; s represents an integer of 0 to 3, preferably 0 or 1.

[0175] In formula (ii-2), R 12b and s R 13b and R 14b The total number of carbon atoms is 25 or less.

[0176] In formula (II), R 1b ~R 10bis a group other than the monovalent sulfur-containing group represented by formula (ii-1) or formula (ii-2), it represents a monovalent group selected from a hydrogen atom, a monovalent hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0177] R 1b ~R 10b When is a monovalent hydrocarbon group, examples of the monovalent hydrocarbon group include linear or branched alkyl groups, linear or branched alkenyl groups, and linear or branched alkynyl groups. Specific examples include methyl, ethane-1-yl, propane-1-yl, 1-methylethane-1-yl, butane-1-yl, butane-2-yl, 2-methylpropane-1-yl, 2-methylpropane-2-yl, pentan-1-yl, pentan-2-yl, hexane-1-yl, heptan-1-yl, octan-1-yl, nonane-1-yl, and decan-1-yl groups. Among these, linear or branched alkyl groups having 1 to 8 carbon atoms are preferred.

[0178] R 1b ~R 10b When is a monovalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, specific examples thereof include those exemplified in the above column of [Substituents, etc.].

[0179] In formula (II), R 1b ~R 10b At least one of the groups is a monovalent sulfur-containing group represented by formula (ii-1) or formula (ii-2). Among them, in consideration of the ease of actual synthesis, cost, heat resistance, or compatibility with the matrix resin being improved, the additive of the present invention can be suppressed from becoming cloudy in the resin member to which it is added, and the additive of the present invention can be added at a high concentration to achieve high ultraviolet absorption ability or high refractive index, R 1b ~R 10b Among these, it is preferable that one or two of them are monovalent sulfur-containing groups represented by formula (ii-1) or formula (ii-2).

[0180] The position of the monovalent sulfur-containing group represented by formula (ii-1) or formula (ii-2) in formula (II) is not particularly limited, but may be any position selected from the group consisting of R 3b or R 8b Examples include: 3. Additive represented by formula (III) The additive represented by the above formula (III) contains a monovalent sulfur-containing group represented by the above formula (iii-1) or (iii-2) in a salicylate-based skeleton.

[0181] In formula (iii-1), R 11c represents a divalent hydrocarbon group having 1 to 12 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0182] R 11c Examples of the divalent hydrocarbon group include linear or branched alkylene groups, alkenylene groups, alkynylene groups, etc. Specific examples include methylene group, ethane-1,2-diyl group, propane-1,3-diyl group, 1-methylethane-1,2-diyl group, butane-1,4-diyl group, butane-1,3-diyl group, 2-methylpropane-1,3-diyl group, pentane-1,5-diyl group, pentane-1,4-diyl group, hexane-1,6-diyl group, heptane-1,7-diyl group, octane-1,8-diyl group, nonane-1,9-diyl group, decane-1,10-diyl group, undecane-1,11-diyl group, dodecane-1,12-diyl group, etc.

[0183] R 11c In the case where a hydrogen atom of the divalent hydrocarbon group is substituted with the monovalent or divalent group, or at least one of the terminals is interrupted, or the carbon-carbon bond is interrupted, the number of the monovalent or divalent groups is preferably 2 or less, and more preferably 1 or less.

[0184] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0185] In formula (iii-1), t represents an integer of 0 or 1.

[0186] In formula (iii-2), R 12c represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0187] R 12c Examples of the divalent hydrocarbon group include linear or branched alkylene groups, linear or branched alkenylene groups, linear or branched alkynylene groups, etc. Specific examples include methylene groups, ethane-1,2-diyl groups, propane-1,3-diyl groups, 1-methylethane-1,2-diyl groups, butane-1,4-diyl groups, butane-1,3-diyl groups, 2-methylpropane-1,3-diyl groups, pentane-1,5-diyl groups, pentane-1,4-diyl groups, hexane-1,6-diyl groups, heptane-1,7-diyl groups, octane-1,8-diyl groups, nonane-1,9-diyl groups, and the like. -diyl group, decane-1,10-diyl group, undecane-1,11-diyl group, dodecane-1,12-diyl group, tridecane-1,13-yl group, tetradecane-1,14-yl group, pentadecane-1,15-yl group, hexadecane-1,16-yl group, heptadecane-1,17-yl group, octadecane-1,18-yl group, nonadecane-1,19-yl group, eicosan-1,20-yl group, etc. Among these, alkylene groups are preferred, and linear alkylene groups are more preferred.

[0188] R 12cIn the case where a hydrogen atom of the divalent hydrocarbon group is substituted with the monovalent or divalent group, or at least one of the terminals is interrupted, or the carbon-carbon bond is interrupted, the number of the monovalent or divalent groups is preferably 2 or less, and more preferably 1 or less.

[0189] Among the monovalent or divalent groups, specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom include those exemplified in the [Substituent, etc.] column.

[0190] In formula (iii-2), R 13c When v is 2 or more, each independently represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0191] R 13c As the divalent hydrocarbon group, R 12c Among these, alkylene groups are preferred, and linear alkylene groups are more preferred.

[0192] R 13c When a divalent hydrocarbon group has a carbon atom substituted with, or at least one of, both ends interrupted, or the carbon-carbon bond interrupted by, said monovalent or divalent group, the number of said monovalent or divalent groups is preferably 2 or less, and more preferably 1 or less.

[0193] Among the monovalent or divalent groups, specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom include those exemplified in the [Substituent, etc.] column.

[0194] In formula (iii-2), R 14crepresents a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, which is a monovalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted.

[0195] R 14c Examples of the monovalent hydrocarbon group include linear or branched alkyl groups, linear or branched alkenyl groups, and linear or branched alkynyl groups. Specifically, for example, methyl group, ethane-1-yl group, propane-1-yl group, 1-methylethane-1-yl group, butane-1-yl group, butane-2-yl group, 2-methylpropane-1-yl group, 2-methylpropane-2-yl group, pentan-1-yl group, pentan-2-yl group, hexane-1-yl group, heptan-1-yl group, octan-1-yl group, nonan-1-yl group, decan-1-yl group, undecane-1-yl group, dodecane-1-yl group, tridecane-1-yl group, tetradecane-1-yl group, pentadecane-1-yl group, hexadecan-1-yl group, heptadecane-1-yl group, octadecane-1-yl group, nonan-1-yl group, eicosan-1-yl group, etc. Among these, alkyl groups are preferred, and linear alkyl groups are more preferred.

[0196] R 14c In the case where a hydrogen atom of the monovalent hydrocarbon group is replaced by the monovalent or divalent group, or at least one of the ends is interrupted, or the carbon-carbon bond is interrupted, the number of the monovalent or divalent groups is preferably 2 or less, and more preferably 1 or less.

[0197] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0198] In formula (iii-2), u represents an integer of 0 or 1; v represents an integer of 0 to 3, preferably 0 or 1.

[0199] In formula (iii-2), R 12c and v R 13c and R 14c The total number of carbon atoms is 25 or less.

[0200] In formula (III), R 1c ~R 10c is a group other than the monovalent sulfur-containing group represented by formula (iii-1) or formula (iii-2), it represents a monovalent group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0201] R 1c ~R 10c When is a monovalent hydrocarbon group, examples of the monovalent hydrocarbon group include linear or branched alkyl groups, linear or branched alkenyl groups, and linear or branched alkynyl groups. Specific examples include methyl, ethane-1-yl, propane-1-yl, 1-methylethane-1-yl, butane-1-yl, butane-2-yl, 2-methylpropane-1-yl, 2-methylpropane-2-yl, pentan-1-yl, pentan-2-yl, hexane-1-yl, heptan-1-yl, octan-1-yl, nonane-1-yl, and decan-1-yl groups. Among these, linear or branched alkyl groups having 1 to 8 carbon atoms are preferred.

[0202] R 1c ~R 10c When is an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, or a halogen atom, specific examples thereof include those exemplified in the above column of [Substituents, etc.].

[0203] In formula (III), R 1c ~R 10cAmong them, at least one of them is a monovalent sulfur-containing group represented by formula (iii-1) or formula (iii-2). Among them, taking into consideration the ease of actual synthesis, cost, heat resistance, and compatibility with the matrix resin to suppress clouding of the resin member to which the additive of the present invention is added, and the ability to express high ultraviolet absorption ability or impart a high refractive index when added at a high concentration, R 1c ~R 10c Among these, it is preferred that one or two of them are monovalent sulfur-containing groups represented by formula (iii-1) or formula (iii-2).

[0204] The position of the monovalent sulfur-containing group represented by formula (iii-1) or formula (iii-2) in formula (III) is not particularly limited, but may be any position selected from the group consisting of R 7c , R 9c Examples include:

[0205] The additives of formulas (II) to (III) incorporating (ii-1) to (iii-1) as monovalent sulfur-containing groups have heat resistance, and can exhibit high ultraviolet absorbing power or impart a high refractive index when added at low to high concentrations. In consideration of this, the monovalent sulfur-containing group represented by formula (ii-1) is preferably such that q is 0 or q is 1 and R 11b contains an alkylene group having 10 or less carbon atoms, and the monovalent sulfur-containing group represented by formula (iii-1) is such that t is 0 or t is 1 and R 11c It is preferred that the alkylene group contains up to 10 carbon atoms.

[0206] The compatibility (transparency) with the matrix resin depends on the number of carbon atoms of the alkyl in the functional groups of formulas (i-v-1) and (i-v-2) in the benzotriazole, benzophenone, salicylate, and triazine skeletons in formulas (I), (II), (III), (IV), and (V) in terms of the additive structure, and on the melting point in terms of physical properties. However, there is no clear correlation between the number of carbon atoms in (i-v-1) and formulas (i-v-2) and the melting point, and it is difficult to achieve both the structure and the physical properties.

[0207] The melting point of these additives tends to decrease when the number of carbon atoms is adjusted by introducing a sulfur-containing group. When the melting point is decreased, the compatibility with the matrix resin becomes particularly good. From this point of view, the monovalent sulfur-containing group represented by formula (ii-1) is such that q is 0 or q is 1 and R 11b contains an alkylene group having 9 or less carbon atoms, and the monovalent sulfur-containing group represented by formula (iii-1) is such that t is 0 or t is 1 and R 11c It is preferable that the compound contains an alkylene group having 9 or less carbon atoms and has a melting point of 91° C. or less under normal pressure (for example, standard atmospheric pressure of 101,325 Pa).

[0208] In another preferred embodiment, the monovalent sulfur-containing group represented by formula (ii-1) is such that q is 0 or q is 1 and R 11b contains an alkylene group having 8 or less carbon atoms, and the monovalent sulfur-containing group represented by formula (iii-1) is such that t is 0 or t is 1 and R 11c contains an alkylene group having 8 or less carbon atoms, and has a melting point of less than 70° C. under normal pressure. Alternatively, the monovalent sulfur-containing group represented by formula (ii-1) is such that q is 0 or q is 1 and R 11b contains an alkylene group having 8 or less carbon atoms, and the monovalent sulfur-containing group represented by formula (iii-1) is such that t is 0 or t is 1 and R 11c contains an alkylene group having 8 or less carbon atoms and has a melting point of 35° C. or less under normal pressure. In other words, when the carbon number is 8 or less and the melting point is less than 70° C., high transparency can be obtained in a thick film thickness even if added at a high concentration, and further, when it is liquid at room temperature (5 to 35° C.), high transparency can be realized in an even thicker film thickness even if added at a high concentration.

[0209] The additives of formulas (II) to (III) incorporating (ii-2) to (iii-2) as monovalent sulfur-containing groups can exhibit high ultraviolet absorbing ability or impart a high refractive index when added at low to high concentrations. In consideration of this, the monovalent sulfur-containing group represented by formula (ii-2) is R 12b and s R 13b and R contains an alkylene group having 18 or less carbon atoms; 14b contains an alkyl group having 18 or less carbon atoms, and the monovalent sulfur-containing group represented by formula (iii-2) is R 12cand v R 13c and R contains an alkylene group having 18 or less carbon atoms; 14c It is preferred that the alkyl group contains up to 18 carbon atoms.

[0210] In addition, when a sulfur-containing group is introduced into these additives to adjust the number of carbon atoms from a short chain to a medium chain, the melting point tends to decrease. When the melting point decreases, the compatibility with the matrix resin becomes particularly good. In consideration of this point, the monovalent sulfur-containing group represented by formula (ii-2) is R 12b and s R 13b and R contains an alkylene group having 18 or less carbon atoms; 14b contains an alkyl group having 18 or less carbon atoms, and the monovalent sulfur-containing group represented by formula (iii-2) is R 12c and v R 13c and R contains an alkylene group having 18 or less carbon atoms; 14c It is preferable that the copolymer contains an alkyl group having 18 or less carbon atoms and has a melting point of 91° C. or less under normal pressure.

[0211] In another preferred embodiment, the monovalent sulfur-containing group represented by formula (ii-2) is R 12b and s R 13b and R contains an alkylene group having 8 or less carbon atoms. 14b contains an alkyl group having 8 or less carbon atoms, and the monovalent sulfur-containing group represented by formula (iii-2) is R 12c and v R 13c and R contains an alkylene group having 8 or less carbon atoms. 14c contains an alkyl group having 8 or less carbon atoms, and has a melting point of less than 70° C. under normal pressure. Alternatively, the monovalent sulfur-containing group represented by formula (ii-2) is 12b and s R 13b and R contains an alkylene group having 8 or less carbon atoms. 14b contains an alkyl group having 8 or less carbon atoms, and the monovalent sulfur-containing group represented by formula (iii-2) is R 12c and v R 13c and R contains an alkylene group having 8 or less carbon atoms. 14ccontains an alkyl group having 8 or less carbon atoms and has a melting point of 35° C. or less under normal pressure. In other words, if the number of carbon atoms is 8 or less and the melting point is less than 70° C., high transparency can be obtained in a thick film thickness even if added at a high concentration, and further, if it is liquid at room temperature (5 to 35° C.), high transparency can be realized even in a thicker film thickness and at a higher concentration. 4. Additive represented by formula (IV) The additive represented by the above formula (IV) contains a monovalent sulfur-containing group represented by the above formula (iv-1) or (iv-2) in a triazine-based skeleton.

[0212] The additive represented by formula (IV) may be either solid or liquid, but when a monovalent sulfur-containing group is introduced, the heat resistance is improved, the compatibility with the matrix resin is particularly good, and high transparency is obtained even when added at a high concentration.

[0213] In formula (iv-1), R 16d represents a divalent hydrocarbon group having 1 to 12 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0214] R 16d Examples of the divalent hydrocarbon group include linear or branched alkylene groups, alkenylene groups, alkynylene groups, etc. Specific examples include methylene group, ethane-1,2-diyl group, propane-1,3-diyl group, 1-methylethane-1,2-diyl group, butane-1,4-diyl group, butane-1,3-diyl group, 2-methylpropane-1,3-diyl group, pentane-1,5-diyl group, pentane-1,4-diyl group, hexane-1,6-diyl group, heptane-1,7-diyl group, octane-1,8-diyl group, nonane-1,9-diyl group, decane-1,10-diyl group, undecane-1,11-diyl group, dodecane-1,12-diyl group, etc.

[0215] R 16dWhen a divalent hydrocarbon group has a carbon atom substituted, a terminal interrupted, or a carbon-carbon bond interrupted by said monovalent or divalent group, the number of said monovalent or divalent groups is preferably 2 or less, more preferably 1 or less.

[0216] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0217] Among these, in consideration of the fact that the compatibility with the matrix resin is good, thereby suppressing clouding of the resin member to which the additive of the present invention is added, and enabling the expression of high ultraviolet absorbing ability or the imparting of a high refractive index when added at a high concentration, divalent hydrocarbon groups having 1 to 9 carbon atoms are preferred, and divalent hydrocarbon groups having 1 to 8 carbon atoms are more preferred. In consideration of this point, an embodiment in which w=0, i.e., formula (iv-1) is -SH, is also preferred. Among the hydrocarbon groups, alkylene groups are preferred, and in a preferred embodiment of the monovalent sulfur-containing group represented by formula (iv-1), w is 0 or w is 1 and R 16d It contains an alkylene group having up to 8 carbon atoms. The alkylene group is particularly preferably a linear alkylene group.

[0218] In formula (iv-1), w represents an integer of 0 or 1.

[0219] In formula (iv-2), R 17d represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted, by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0220] R 17dExamples of the divalent hydrocarbon group include linear or branched alkylene groups, linear or branched alkenylene groups, linear or branched alkynylene groups, etc. Specific examples include methylene groups, ethane-1,2-diyl groups, propane-1,3-diyl groups, 1-methylethane-1,2-diyl groups, butane-1,4-diyl groups, butane-1,3-diyl groups, 2-methylpropane-1,3-diyl groups, pentane-1,5-diyl groups, pentane-1,4-diyl groups, hexane-1,6-diyl groups, heptane-1,7-diyl groups, octane-1,8-diyl groups, nonane-1,9-diyl groups, and the like. -diyl group, decane-1,10-diyl group, undecane-1,11-diyl group, dodecane-1,12-diyl group, tridecane-1,13-yl group, tetradecane-1,14-yl group, pentadecane-1,15-yl group, hexadecane-1,16-yl group, heptadecane-1,17-yl group, octadecane-1,18-yl group, nonadecane-1,19-yl group, eicosan-1,20-yl group, etc. Among these, alkylene groups are preferred, and linear alkylene groups are more preferred.

[0221] R 17d When a divalent hydrocarbon group has a hydrogen atom substituted, a base end interrupted, or a carbon-carbon bond interrupted by said monovalent or divalent group, the number of said monovalent or divalent groups is preferably 2 or less, and more preferably 1 or less.

[0222] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0223] In formula (iv-2), R 18d When y is 2 or more, each independently represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, at least one of both ends may be interrupted, or the carbon-carbon bond may be interrupted by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0224] R18d As the divalent hydrocarbon group, R 17d Among these, alkylene groups are preferred, and linear alkylene groups are more preferred.

[0225] R 18d When a divalent hydrocarbon group has a hydrogen atom substituted, a base end interrupted, or a carbon-carbon bond interrupted by said monovalent or divalent group, the number of said monovalent or divalent groups is preferably 2 or less, and more preferably 1 or less.

[0226] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0227] In formula (iv-2), R 19d represents a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, which is a monovalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted, the group end may be interrupted, or the carbon-carbon bond may be interrupted.

[0228] R 19dExamples of the monovalent hydrocarbon group include linear or branched alkyl groups, linear or branched alkenyl groups, and linear or branched alkynyl groups. Specifically, for example, methyl group, ethane-1-yl group, propane-1-yl group, 1-methylethane-1-yl group, butane-1-yl group, butane-2-yl group, 2-methylpropane-1-yl group, 2-methylpropane-2-yl group, pentan-1-yl group, pentan-2-yl group, hexane-1-yl group, heptan-1-yl group, octan-1-yl group, nonan-1-yl group, decan-1-yl group, undecane-1-yl group, dodecane-1-yl group, tridecane-1-yl group, tetradecane-1-yl group, pentadecane-1-yl group, hexadecan-1-yl group, heptadecane-1-yl group, octadecane-1-yl group, nonan-1-yl group, eicosan-1-yl group, etc. Among these, alkyl groups are preferred, and linear alkyl groups are more preferred.

[0229] R 19d When the monovalent hydrocarbon group has a hydrogen atom substituted, a base end interrupted, or a carbon-carbon bond interrupted by said monovalent or divalent group, the number of substituents is preferably 2 or less, more preferably 1 or less.

[0230] Specific examples of the aromatic group, unsaturated group, sulfur-containing group, oxygen-containing group, phosphorus-containing group, alicyclic group, and halogen atom of the monovalent or divalent group include those exemplified in the [Substituent, etc.] column.

[0231] In formula (iv-2), x represents an integer of 0 or 1; y represents an integer of 0 to 3, preferably 0 or 1.

[0232] In formula (iv-2), R 17d and y R 18d and R 19dThe total number of carbon atoms in is preferably 54 or less, more preferably 36 or less, and particularly preferably 25 or less. Among these, the monovalent sulfur-containing group represented by formula (iv-2) is preferably R 17d and y R 18d and R contains an alkylene group having 18 or less carbon atoms; 19d is preferably an alkyl group having 18 or less carbon atoms, and R 17d and y R 18d and R contains an alkylene group having 12 or less carbon atoms; 19d is preferably an alkyl group having 12 or less carbon atoms, and R 17d and y R 18d and R contains an alkylene group having 8 or less carbon atoms. 19d is particularly preferably an alkyl group having 8 or less carbon atoms. 17d and y R 18d and R 19d are linear and R 17d , R 18d , R 19d Each of R preferably has 1 to 18 carbon atoms. 17d , R 18d , R 19d More preferably, each of R has 1 to 12 carbon atoms. 17d , R 18d , R 19d Each of these more preferably has 1 to 8 carbon atoms, even more preferably has 1 to 6 carbon atoms, and particularly preferably has 1 carbon atom (this also includes the cases where x=0 and y=0).

[0233] In formula (IV), R 1d ~R 15d is a group other than the monovalent sulfur-containing group represented by formula (iv-1) or formula (iv-2), it represents a monovalent group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0234] R1d ~R 15d When is a monovalent hydrocarbon group, examples of the monovalent hydrocarbon group include linear or branched alkyl groups, linear or branched alkenyl groups, and linear or branched alkynyl groups. Specific examples include methyl, ethane-1-yl, propane-1-yl, 1-methylethane-1-yl, butane-1-yl, butane-2-yl, 2-methylpropane-1-yl, 2-methylpropane-2-yl, pentan-1-yl, pentan-2-yl, hexane-1-yl, heptan-1-yl, octan-1-yl, nonane-1-yl, and decan-1-yl groups. Among these, linear or branched alkyl groups having 1 to 8 carbon atoms are preferred.

[0235] R 1d ~R 15d When is a monovalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, specific examples thereof include those exemplified in the above column of [Substituents, etc.].

[0236] In formula (IV), R 1d ~R 15d Among them, at least one of them is a monovalent sulfur-containing group represented by formula (iv-1) or formula (iv-2). Among them, taking into consideration the ease of actual synthesis, cost, heat resistance, and compatibility with the matrix resin being improved, the opacity of the resin member to which the additive of the present invention is added is suppressed, and the addition of a high concentration makes it possible to express high ultraviolet absorbing ability or impart a high refractive index, R 1d ~R 15d Among these, it is preferable that 1 to 3 are monovalent sulfur-containing groups represented by formula (iv-1) or formula (iv-2).

[0237] The position of the monovalent sulfur-containing group represented by formula (iv-1) or formula (iv-2) in formula (IV) is not particularly limited, but may be any position selected from the group consisting of R 3d , R 8d , R 13d Some examples include: The triazine skeleton contains a monovalent sulfur-containing group represented by the above formula (iv-1) or (iv-2). 5. Additive represented by formula (V) The additive represented by the above formula (V) contains a long-chain alkyl group in a benzotriazole-based skeleton.

[0238] In formula (V), R 1e ~R 9e At least one of these is an alkyl group having 10 to 24 carbon atoms. This alkyl group having 10 to 24 carbon atoms has a straight chain having 10 to 20 carbon atoms, and the straight chain may be substituted with up to two alkyl groups each having 1 or 2 carbon atoms. Among these, a straight chain alkyl group is preferred.

[0239] Specific examples of the alkyl group having 10 to 24 carbon atoms include decan-1-yl, undecane-1-yl, dodecane-1-yl, tridecane-1-yl, tetradecane-1-yl, pentadecane-1-yl, hexadecan-1-yl, heptadecan-1-yl, octadecane-1-yl, nonan-1-yl, eicosan-1-yl, henicosan-1-yl, docosan-1-yl, tricosan-1-yl, and tetracosan-1-yl groups.

[0240] In formula (V), R 1e ~R 9e When represents a group other than the alkyl group having 10 to 24 carbon atoms, it represents a monovalent group selected from a hydrogen atom, a hydrocarbon group having 1 to 4 carbon atoms, an aromatic group, an unsaturated group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom.

[0241] R 1e ~R 9eWhen is a monovalent hydrocarbon group, examples of the monovalent hydrocarbon group include linear or branched alkyl groups, linear or branched alkenyl groups, linear or branched alkynyl groups, etc. Specific examples include methyl group, ethane-1-yl group, propan-1-yl group, 1-methylethane-1-yl group, butan-1-yl group, butan-2-yl group, 2-methylpropan-1-yl group, 2-methylpropan-2-yl group, etc.

[0242] R 1e ~R 9e When is an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, or a halogen atom, specific examples thereof include those exemplified in the above column of [Substituents, etc.].

[0243] In formula (V), R 1e ~R 9e At least one of the above is an alkyl group having 10 to 24 carbon atoms. Among them, taking into consideration the ease and cost of actual synthesis, or the fact that the additive of the present invention can be added to a resin member by improving compatibility with the matrix resin, thereby suppressing clouding, and enabling the expression of high ultraviolet absorbing ability or the imparting of a high refractive index when added at a high concentration, R 1e ~R 9e Of these, it is preferable that one or two are the above-mentioned alkyl groups having 10 to 24 carbon atoms.

[0244] The position of the alkyl group having 10 to 24 carbon atoms in the formula (V) is not particularly limited, but R 2e or R 4e etc.

[0245] In the present invention, the following points are taken into consideration regarding the relationship between the ability to increase the compatibility between the additive and the resin and the melting point of the additive. When the interaction between the molecules of the additive is large, the interaction between the molecules of the additive and the molecules of the resin is difficult, and the compatibility between them decreases. On the other hand, when the interaction between the molecules of the additive is large, the melting point of the additive increases. In other words, the melting point of the additive is an index of the interaction between the molecules of the additive and further the compatibility between the additive and the resin, and it is presumed that the introduction of a sulfur-containing group or an appropriately selected alkyl group into the additive can reduce the interaction between the molecules of the additive (lower the melting point) and increase the compatibility between the additive and the resin.

[0246] The additive of the present invention exerts ultraviolet absorbing ability by the ultraviolet absorbing skeleton such as benzotriazole, has an ultraviolet absorption band in the vicinity of 250 to 400 nm, cuts the wavelength of the ultraviolet region, and transmits the wavelength of the visible light region. There is a demand for an ultraviolet absorber that can absorb up to the UV-A region (315 to 400 nm) that affects the photodegradation of all organic substances, but the additive of the present invention has excellent ultraviolet absorbing ability in the UV-A region, and depending on the chemical structure, it is possible to cut ultraviolet rays up to the region around 400 nm. In addition, by introducing functional groups i to iv-1, 2, not only can the refractive index be increased, but the region of the ultraviolet absorption band can be adjusted and the function can be improved. The additive of the present invention, in which a benzotriazole group of a benzotriazole compound or a thioether group (i-2, iv-2) is introduced into a triazine compound, shifts the wavelength to a long wavelength without cutting 450 to 500 nm (visible region), and can cut ultraviolet rays of a longer wavelength around 360 to 400 nm even in the UV-A region. On the other hand, the additive of the present invention, in which a thioether group (i-2) is introduced into the phenyl group on the nitrogen of a benzotriazole-based compound, can shift the absorption band to a shorter wavelength and have an absorption band in the short wavelength region around 290 nm. Furthermore, the additive of the present invention, in which one thioether group (iv-2) is introduced into a triazine-based compound of the present invention, has an ultraviolet absorption band in the short wavelength ultraviolet region of 260 to 280 nm in addition to the long wavelength region around 360 to 400 nm, making it possible to absorb ultraviolet rays over a wider range.

[0247] The additive of the present invention can maintain the transparency of a resin when added to the resin, and since the additive of the present invention has excellent heat resistance, it is not easily thermally decomposed during the process of hot molding and processing a resin workpiece containing the additive, so that a resin workpiece can be obtained that does not lose its appearance, its ultraviolet absorbing ability and its high refractive index, and further, in the case of a transparent resin workpiece, a highly transparent workpiece can be obtained.

[0248] Also, R 6a ~R 9a A transparent resin workpiece containing the additive of the present invention represented by formula (I) in which a thioether group i-2 has been introduced, not only achieves the transparency and high refractive index of the resin due to the heat resistance and compatibility of the additive with the resin, but also enables absorption of wavelengths in the long wavelength region while suppressing yellowing due to the characteristics of the ultraviolet absorption peak.

[0249] On the other hand, the additives of the present invention represented by formulas (I) to (V) having reactive functional groups such as hydroxyl groups, thiol groups, carboxyl groups, amino groups, and silyl groups, including polymerizable functional groups and crosslinkable functional groups such as vinyl groups, vinyloxy groups, allyl groups, (meth)acryloyl groups, maleoyl groups, styryl groups, and cinnamoyl groups in the thiol groups i to iv-1 and the thioether groups i to iv-2, can react with functional groups that react with those functional groups (for example, isocyanate groups, epoxy groups, carboxyl groups, carbonyl groups, hydroxyl groups, When a resin part is obtained by reacting, copolymerizing, or molding raw material monomers and resins for a film and a resin part containing functional groups such as aryl groups, alkoxy groups, alkenyl groups, alkynyl groups, ether groups, thioisocyanate groups, thioepoxy groups, thiocarboxylate groups, thiocarbonyl groups, and thiol groups, the above-mentioned additives copolymerize with the monomers or react with the functional groups of the resin and are fixed in the matrix, retaining transparency without bleeding out, and being able to retain their respective ultraviolet absorption capabilities and high refractive index functions for a long period of time.

[0250] The introduction of the sulfur-containing group improves the refractive index, and a high refractive index can be imparted to the resin member. The refractive index of the additive of the present invention is not particularly limited, but is, for example, 1.55 or more, preferably 1.58 to 1.62, and more preferably 1.60 to 1.62.

[0251] The additive of the present invention has a sulfur-containing group, particularly a sulfur-containing group having a short- to medium-chain hydrocarbon as a spacer, introduced into the ultraviolet absorbing skeleton of a benzotriazole system or the like, and thus has improved compatibility with resin members, and can be dissolved at a high concentration of 0.4 wt% or more, further 10 wt% or more, particularly 30 wt% or more while maintaining high transparency. Therefore, it is possible to impart at least one of high ultraviolet absorption ability and high refractive index while maintaining high transparency. That is, it is possible to dissolve at a high concentration in resin members that could not be dissolved at a high concentration with existing ultraviolet absorbers and refractive index improvers, and it is possible to impart a transparent, higher ultraviolet absorption ability or high refractive index to the resin member.

[0252] Among these, when the melting point of the additive of the present invention is less than 70°C, or even when the additive is liquid at room temperature of 35°C or less, the compatibility with resin components is particularly good, and in particular, when benzotriazole, benzophenone, or salicylate-based additives are added at a high concentration of 50 wt% or more, high transparency can be obtained in the matrix.

[0253] Furthermore, by adding only one additive to one film or sheet, it is possible to impart both ultraviolet absorbing ability and a high refractive index to the matrix. For example, in a film or member having a functional optical layer such as a multilayer optical film, it is possible to combine two layers (an ultraviolet absorbing layer and a high refractive index layer) into one layer by using only one additive.

[0254] When producing the additives represented by formulae (I) to (V), reference is made to the disclosure of the Examples described below and known techniques. 6. Resin parts using the additive of the present invention The resin member of the present invention contains the additive of the present invention described above.

[0255] The shape of the resin member of the present invention is not particularly limited and may be any shape, but since it is possible to impart high ultraviolet absorption ability and / or high refractive index while maintaining transparency, the laminated multilayer structure is simplified, and the manufacturing process and costs can be reduced. In particular, one layer of a member having a multilayer structure, a film or sheet having flexibility or flexibility, or a rigid In addition, optical molded products, for example, optical lenses such as lens elements for glasses and contact lenses, are preferred.

[0256] A resin workpiece containing the additive of the present invention can maintain the transparency of the resin, and since the additive of the present invention has excellent heat resistance, the resin workpiece containing the additive is not easily thermally decomposed during the process of hot molding and processing. This means that the appearance of the resin workpiece is not impaired, and the ultraviolet absorbing ability and high refractive index of the resin workpiece are not reduced, and further, in the case of transparent parts, a highly transparent part can be obtained.

[0257] Also, R 6a ~R 9aThe transparent resin workpieces containing the additives of the present invention represented by formulas (I) to (V) in which a thioether group of iv-2 has been introduced, not only achieve the transparency and high refractive index of the resin due to the heat resistance and compatibility of the additives with the resin, but also enable absorption of wavelengths in the long wavelength region while suppressing yellowing due to the characteristics of the ultraviolet absorption peak. In addition, when a resin member containing the additive of the present invention represented by formula (I) to formula (V) having reactive functional groups such as thiol groups, vinyl groups, and hydroxyl groups in the thiol groups i to iv-1 and the thioether groups i to iv-2 contained in the additives is reacted and molded using raw material monomers and resins for the film and resin member containing functional groups (e.g., isocyanate groups, epoxy groups, carboxyl groups, carbonyl groups, hydroxyl groups, alkenyl groups, alkynyl groups, ether groups, thioisocyanate groups, thioepoxy groups, thiocarboxyl groups, thiocarbonyl groups, thiol groups, etc.) that react with reactive functional groups such as thiol groups, vinyl groups, and hydroxyl groups contained in the additives, the resulting resin has the above-mentioned additives reacting with the functional groups of the monomers and resins and being fixed in the matrix, and can retain their respective ultraviolet absorbing ability and high refractive index functions for a long period of time without bleeding out.

[0258] R in formula (I) 6a ~R 9a The transparent resin workpiece containing the additive of the present invention, which has a substituent represented by formula (i-1) or formula (i-2) introduced therein, maintains transparency and a high refractive index, and furthermore, due to the ultraviolet absorbing property of the additive, it is possible to sharply cut ultraviolet rays of longer wavelengths around 360 to 400 nm even in the UV-A region without cutting 450 to 500 nm (visible region). Therefore, the resin workpiece obtained has excellent appearance with suppressed yellow coloring.

[0259] The resin member of the present invention is not particularly limited, and examples thereof include acrylic resins such as polymethyl(meth)acrylate, polyethyl(meth)acrylate, and methyl(meth)acrylate-butyl(meth)acrylate copolymers; polyolefin resins such as polyethylene, polypropylene, polymethylpentene, and cyclic olefin polymers; thermoplastic polyester resins such as polycarbonate resins, polyethylene terephthalate, and polyethylene naphthalate; cellulose resins such as polyurethane, polythiourethane, polystyrene, polyamide, polyimide, acrylonitrile-styrene copolymers, polyethersulfone, polysulfone, and triacetyl cellulose; polyvinyl acetate, ethylene-vinyl acetate copolymers, polyvinylpyrrolidone, polyvinyl chloride, polyvinylidene chloride, and polyether Examples of the resin include thermoplastic resins such as ether ketone, polyacetal, and nylon; thermosetting resins such as urethane, thiourethane, urea, melamine, acrylic melamine, episulfide, epoxy, allyl, silicone, phenol, urea, and unsaturated polyester; acrylic, for example, monofunctional or polyfunctional (meth)acrylate compounds such as acrylic acid of a polyhydric alcohol, 2-hydroxyethyl methacrylate, or methacrylic acid ester; polyfunctional urethane (meth)acrylate compounds synthesized from a diisocyanate, a polyhydric alcohol, and a hydroxy ester of acrylic acid or methacrylic acid; and ultraviolet-curable resins such as polyether, polyester, epoxy, alkyd, spiroacetal, polybutadiene, and polythiolpolyene having an acrylate functional group.

[0260] The resin member of the present invention can be produced, for example, by the following methods (1) to (4), although the method is not particularly limited. (1) A method of applying a coating liquid containing the additive of the present invention and a resin or raw material monomer to a substrate, and forming a film by heating, irradiating with ultraviolet rays, or drying. (2) A method in which the additive of the present invention is mixed and kneaded into a resin or a raw material monomer, and then molded into a film using an extruder or the like. (3) A method in which the additive of the present invention is incorporated into a resin adhesive and the resin adhesive is applied to a film. (4) A method in which the additive of the present invention is dissolved in a raw material monomer, poured into a metal mold or glass mold, and hardened and molded by heating, irradiating with ultraviolet light, or drying. Among these methods, the method (1) of applying a coating liquid containing the additive of the present invention and a resin or raw monomer material to form a film is preferred in the present invention from the viewpoint of obtaining a transparent multilayer structure, film, or sheet.

[0261] In this method, the additive of the present invention and the resin or raw material monomer are diluted in an organic solvent or aqueous solvent, or not diluted, to prepare a coating liquid, which is then applied to a substrate to form a film. If necessary, drying, cooling, heating, or ultraviolet irradiation are performed to improve the film strength.

[0262] The resin is not particularly limited, and can be appropriately selected in consideration of the necessary physical properties such as adhesion to the substrate and hardness, for example, as long as it is a film or member having a functional optical layer. Specific examples include ultraviolet-curable resins, electron beam-curable resins, thermosetting resins, and thermoplastic resins. More specific examples include polyester resins, acrylic resins, urethane resins, thiourethane resins, polyethylene terephthalate resins, polystyrene resins, polycarbonate resins, urea resins, melamine resins, acrylic melamine resins, epoxy resins, alkyd resins, spiroacetal resins, polybutadiene resins, polyolefin resins, polyvinyl resins, polyvinyl alcohol resins, polyvinyl-modified resins (PVB, EVA, etc.), silicone resins, polyamide resins, polyether resins, episulfide resins, nylon resins, or copolymer resins thereof.

[0263] In films or members having a functional optical layer, ultraviolet curing resins, electron beam curing resins, thermosetting resins, thermoplastic resins, etc. can be used. A coating liquid containing these resins is applied to a transparent substrate to form a coating film, and this coating film is dried as necessary. Thereafter, the coating film is irradiated with ultraviolet rays or electron beams or heated to cause a curing reaction, thereby forming a transparent optical layer.

[0264] The ultraviolet curing resin may be an acrylic material. For example, a monofunctional or polyfunctional (meth)acrylate compound such as acrylic acid or methacrylic acid ester, or a polyfunctional urethane (meth)acrylate compound synthesized from a diisocyanate, a polyhydric alcohol, and a hydroxy ester of acrylic acid or methacrylic acid may be used. In addition to these, polyether resins, polyester resins, epoxy resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiol polyene resins, and the like having acrylate functional groups may also be used.

[0265] When using an ultraviolet-curing resin, a photopolymerization initiator is added to the coating liquid. The photopolymerization initiator may be any that generates radicals when irradiated with ultraviolet light. For example, acetophenones, benzoins, benzophenones, phosphine oxides, ketals, anthraquinones, thioxanthones, etc. may be used.

[0266] As the thermosetting resin, for example, a urethane resin, a thiourethane resin, a melamine resin, an acrylic melamine resin, a urea resin, a phenol resin, an epoxy resin, an episulfide resin, or the like can be used.

[0267] Examples of the thermoplastic resin that can be used include urethane resin, thiourethane resin, polyethylene terephthalate resin, polystyrene resin, polycarbonate resin, polyester resin, polyethylene resin, polypropylene resin, acrylic resin, and nylon resin.

[0268] If necessary, a solvent for dilution may be added to the coating liquid. Examples of the solvent include aromatic hydrocarbons such as toluene, xylene, cyclohexane, and cyclohexylbenzene; hydrocarbons such as n-hexane; ethers such as dibutyl ether, dimethoxymethane, dimethoxyethane, diethoxyethane, propylene oxide, dioxane, dioxolane, trioxane, tetrahydrofuran, anisole, and phenetole; ketones such as methyl isobutyl ketone, methyl butyl ketone, acetone, methyl ethyl ketone, diethyl ketone, dipropyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, and methylcyclohexanone; esters such as ethyl formate, propyl formate, n-pentyl formate, methyl acetate, ethyl acetate, methyl propionate, ethyl propionate, n-pentyl acetate, and γ-butyrolactone; cellosolves such as methyl cellosolve, cellosolve, butyl cellosolve, and cellosolve acetate; alcohols such as methanol, ethanol, and isopropyl alcohol; and water.

[0269] The coating liquid may contain additives such as antifoaming agents, leveling agents, antioxidants, light stabilizers, polymerization inhibitors, catalysts, dyes, and pigments, if necessary.

[0270] The amount of the additive of the present invention used is not particularly limited, taking into consideration ultraviolet absorbing ability, high refractive index, transparency, etc., depending on the purpose, but can be added in an amount of 0.4 wt% or more, further 10 wt% or more, further 30 wt% or more, and particularly 50 wt% or more based on the total amount of the coating liquid excluding volatile components such as solvents. Even when added at such a high concentration, the additive of the present invention dissolves uniformly in the resin that becomes the matrix, and can maintain high transparency.

[0271] The prepared coating liquid can be applied to a substrate by an appropriate method such as a bar coater, gravure coater, comma coater, lip coater, curtain coater, roll coater, blade coater, spin coater, reverse coater, die coater, spraying, or dipping.

[0272] The substrate for coating is not particularly limited, but examples thereof include resin plates, resin films, resin sheets, glass, building materials, and the like.

[0273] When the resin member of the present invention is used as a part of a film or member having a functional optical layer such as an anti-reflection film, the material can be selected as a substrate for coating in consideration of optical properties such as transparency and refractive index of light, as well as various physical properties such as impact resistance, heat resistance, and durability. Such materials are not particularly limited, but include acrylic resins such as poly(methyl meth)acrylate, poly(ethyl meth)acrylate, and methyl (meth)acrylate-butyl (meth)acrylate copolymers, polyolefin resins such as polyethylene, polypropylene, polymethylpentene, and cyclic olefin polymers, thermoplastic polyester resins such as polycarbonate resins, polyethylene terephthalate, and polyethylene naphthalate, cellulose resins such as polyamide, polyimide, polystyrene, acrylonitrile-styrene copolymers, polyethersulfone, polysulfone, and triacetyl cellulose, thermoplastic resin materials such as polyvinyl acetate, ethylene-vinyl acetate copolymers, polyvinyl chloride, polyvinylidene chloride, polyether ether ketone, and polyurethane, or glass (including ceramics) such as soda glass, potash glass, and lead glass, and light-transmitting inorganic materials such as quartz, fluorite, and diamond.

[0274] These materials may contain known additives, such as ultraviolet absorbing agents, infrared absorbing agents, and high refractive index agents. Other additives may also be added, such as plasticizers, lubricants, colorants, antioxidants, and flame retardants.

[0275] When used as a film having a functional optical layer, the thickness of the substrate is not particularly limited, but is, for example, 50 nm to 150 μm. Such a substrate may be a single layer or a laminate of multiple layers.

[0276] Furthermore, among the above-mentioned methods for producing the resin member of the present invention, in the method (2) in which the additive of the present invention is mixed and kneaded into a resin and then molded and made into a film using an extruder or the like, the additive of the present invention can be added to powder or pellets of a resin, heated and dissolved, and then molded to produce the resin member.

[0277] The resin powder or pellets are not particularly limited, and examples thereof include acrylic resins such as polymethyl(meth)acrylate, polyethyl(meth)acrylate, and methyl(meth)acrylate-butyl(meth)acrylate copolymers; polyolefin resins such as polyethylene, polypropylene, polymethylpentene, and cyclic olefin polymers; thermoplastic polyester resins such as polycarbonate resin, polyethylene terephthalate, and polyethylene naphthalate; cellulose resins such as polyamide, polyimide, polystyrene, acrylonitrile-styrene copolymer, polyethersulfone, polysulfone, and triacetyl cellulose; and thermoplastic resin materials such as polyvinyl acetate, ethylene-vinyl acetate copolymer, polyvinylpyrrolidone, polyvinyl chloride, polyvinylidene chloride, polyether ether ketone, polyacetal, nylon, and polyurethane.

[0278] The method for molding the resin member is not particularly limited, and can be injection molding, extrusion molding, calendar molding, blow molding, compression molding, etc. When an extruder is used, the resin member can be produced by forming a film using the extruder, or by producing a raw material using the extruder and then stretching it uniaxially or biaxially to form a film.

[0279] The additive of the present invention has improved heat resistance by introducing a thioether group. The 5% weight loss temperature of the additive of the present invention is higher than the softening temperature of general resins, which is 100 to 250°C ("Easy to Understand Plastics", supervised by the Japan Plastics Industry Federation, published by Nihon Jitsugyo Publishing Co., Ltd.), and therefore can be applied to thermosetting resins and thermoplastic resins with molding temperatures of 100 to 200°C, as well as thermoplastic resins that require molding temperatures higher than 200 to 250°C.

[0280] During kneading, additives typically used in resin molding, such as infrared absorbing agents, ultraviolet absorbing agents, high refractive index agents, antioxidants, light stabilizers, flame retardants, and plasticizers, may be added.

[0281] Furthermore, among the above-mentioned methods for producing the resin member of the present invention, in the method (3) in which the additive of the present invention is incorporated into a resin adhesive and the resin adhesive is applied to a film, a known transparent adhesive such as a commonly used silicone-based, urethane-based, acrylic-based, polyvinyl butyral adhesive (PVB), ethylene-vinyl acetate-based, or epoxy-based adhesive is used as the resin adhesive, and a composite material including the resin member of the present invention can be produced by bonding and curing resin films together using the resin adhesive containing the additive of the present invention.

[0282] When the resin workpiece of the present invention is used as a part of a film or workpiece having a functional optical layer, the film thickness is not particularly limited as long as it is within a range that satisfies the required physical properties such as the type of resin material, adhesion, hardness, etc., and is, for example, within a range of 50 nm to 200 μm.

[0283] In the above-mentioned method for producing the resin member of the present invention, in the method (4) in which the additive of the present invention is dissolved in a raw material monomer, cast into a metal mold or glass mold, and cured by heating, ultraviolet irradiation, or drying to form a mold, a thermosetting resin monomer can be used in the case of curing by heating, and is not particularly limited. For example, a resin raw material monomer capable of producing urethane, thiourethane, epoxy, thioepoxy, melamine, silicone, phenol, urea, or unsaturated polyester resin can be used. The additive of the present invention is dissolved in at least one monomer among the resin raw material monomers, and other resin monomers required for resinification are mixed, and then the mixture is cast into a metal mold or glass mold and heated to produce a resin member containing the additive of the present invention. An acrylic material can be used as the ultraviolet curing resin. As the acrylic material, a monofunctional or polyfunctional (meth)acrylate compound such as acrylic acid, 2-hydroxyethyl methacrylate, or methacrylic acid ester, or a polyfunctional urethane (meth)acrylate compound synthesized from a diisocyanate, a polyhydric alcohol, and a hydroxyester of acrylic acid or methacrylic acid, etc. can be used. In addition to these, polyether resins, polyester resins, epoxy resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiolpolyene resins, and the like having acrylate functional groups can also be used.

[0284] The resin member of the present invention can be used in all applications where synthetic resins are used, and is particularly suitable for applications where there is a possibility of exposure to sunlight or light including ultraviolet light, although there is no particular limitation thereto. Examples of such applications include glass substitutes, coating agents and protective agents for glass such as window glass, lighting glass, and light source protection glass, light source members that emit ultraviolet light such as fluorescent lamps and mercury lamps, containers or packaging materials for food and medicine, agricultural and industrial sheets, printed matter, dyed matter, dyes and pigments, display boards, indicator lights, cards, and other discoloration prevention agents.

[0285] In particular, the resin workpiece of the present invention is particularly suitable for optical materials, particularly films and members having functional optical layers, and optical molded products, because it is possible to impart ultraviolet absorption ability and a high refractive index while maintaining the transparency of the matrix.

[0286] The film or member having a functional optical layer may be a monolayer film, or a multilayer film or substrate having an optical layer in which one or more optical layers are provided on a base film or substrate according to various applications. When multiple optical layers are provided, the resin member of the present invention is used for at least one of the layers.

[0287] Among the films and members having a functional optical layer, the optical film may be a base film having a functional layer for various applications, and examples thereof include various optical disk substrate protective films, reflective films, anti-reflective films, alignment films, polarizing films, polarizing layer protective films, retardation films, light diffusion films, viewing angle improving films, electromagnetic wave shielding films, anti-glare films, light shielding films, and brightness improving films.

[0288] Examples of members having a functional optical layer include members in which at least one of an antireflection layer, a hard coat layer, an antistatic layer, an adhesion stabilizing layer, a protective layer, an electromagnetic wave shielding layer, an infrared ray cutting layer, etc. is laminated in one or more layers on the surface of a panel substrate or the like.

[0289] The resin member of the present invention is also suitable for a surface protective film for a solar cell. A solar cell element is usually configured with an active layer acting as a solar cell between a pair of substrates, but a flexible solar cell requires an ultraviolet absorbing protective film because polyester materials such as gas barrier films used as its members, and the active layer itself in an organic solar cell, absorb ultraviolet light and deteriorate. In addition, since solar cells are installed outdoors for many years, such protective films are required to have high weather resistance. Furthermore, since solar cells absorb light energy and convert it into electricity, such protective films are required to have high transparency. That is, a protective film for protecting a flexible solar cell is required to have high transparency, high ultraviolet absorbing ability, high weather resistance, and flexibility, and the resin member of the present invention is suitable for such applications.

[0290] The resin member of the present invention can be suitably used for optical lenses such as plastic lens elements for spectacles, contact lenses, optical pickup lenses, camera lenses, and lenticular lenses, prisms, filters, optical substrates such as touch panel substrates and light guide plates, optical fibers, information recording substrates, and other optical molded products. As optical lenses, the resin member is also suitable for plastic lenses such as lens films such as Fresnel lens films and lenticular lens films, and microlens arrays using microlenses with a diameter of several μm, which are used for the purpose of increasing the light collecting and light diffusing properties of miniaturized optical functional elements or for the purpose of collecting light on the light receiving elements of image pickup elements.

[0291] The resin member of the present invention is also suitable as a display substrate, for example, a substrate for flat panel displays such as liquid crystal displays, organic EL displays, plasma displays, field emission displays, and electronic paper, or a substrate for backlights such as liquid crystal displays, traffic lights, and neon signs.

[0292] When absorbing ultraviolet rays in a wide range of wavelengths with a resin member such as a film, it is necessary to use multiple additives, add the additives at high concentrations, or make the film or resin thick, but in such cases, problems are likely to occur in terms of transparency and coloring. However, the triazine-based compound with one thioether group introduced therein used in the additive of the present invention has an ultraviolet absorption band in the long wavelength region of 360 to 400 nm and the short wavelength ultraviolet region of 260 to 280 nm, making it possible to absorb ultraviolet rays in a wider range, and one additive can absorb ultraviolet rays in a wide range of wavelengths at a low concentration.

[0293] For example, in a light-shielding film, it is desirable to cut ultraviolet rays from 360 to 400 nm, but general additives cut only up to 450 to 500 nm (visible range), which causes problems such as reduced visible light and discoloration. However, the additive of the present invention, which has a benzotriazole group in a benzotriazole compound or a thioether group (i-2, iv-2) introduced into a triazine compound, can cut ultraviolet rays of 360 to 400 nm, which is a longer wavelength, even in the 315 to 400 nm (UV-A region) without cutting 450 to 500 nm (visible range), and is highly useful.

[0294] The additive of the present invention, which has an ultraviolet absorption peak top in the short wavelength region around 290 nm and in which a thioether group i-2 has been introduced into the phenyl group on the nitrogen of a benzotriazole compound, can effectively prevent deterioration of resins that deteriorate at wavelengths around 290 to 300 nm, such as polyethylene, polymethyl methacrylate, and polycarbonate.

[0295] Furthermore, the additive of the present invention can be used not only in films and resin members, but also in, for example, dyes, pigments, dyes, inks, paints, pharmaceuticals, surface coatings, cosmetics, photographic materials, textiles, etc., which are required to be stabilized and functionalized by an ultraviolet absorber while having the above-mentioned functions. EXAMPLES

[0296] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples in any way. <Synthesis Example 1> Synthesis of intermediate 1

[0297] [ka]

[0298] Dibromohexane (50.0g, 204.9mmol) and potassium thioacetate (10.6g, 102.5mmol) were heated under reflux in 150mL of acetonitrile for 6 hours. After the reaction was completed, the solid formed was filtered off, and the solvent was distilled off from the filtrate to obtain a liquid crude product. The crude product was then purified using a column to obtain intermediate 1 as a transparent liquid. <Synthesis Example 2> Synthesis of intermediate 2

[0299] [ka]

[0300] Dibromodecane (50.0g, 166.6mmol) and potassium thioacetate (8.6g, 83.3mmol) were heated under reflux in 150mL of acetonitrile for 6 hours. After the reaction was completed, the solid formed was filtered off, and the solvent was distilled off from the filtrate to obtain a liquid crude product. The crude product was then purified using a column to obtain intermediate 2 as a transparent liquid. <Synthesis Example 3> Synthesis of intermediate 3

[0301] [ka]

[0302] Octanethiol (29.3g, 200mmol) and 55% sodium hydride (13.1g, 300mmol) were stirred in 150ml of THF under ice cooling for 2 hours, and the resulting suspension was then added dropwise to 100mL of a THF solution of dibromopropane (121.1g, 600mmol) under ice cooling and reacted for 2 hours. After adding toluene and washing with water, intermediate 3 was obtained by distillation under reduced pressure. <Synthesis Example 4> Synthesis of intermediate 4

[0303] [ka]

[0304] Intermediate 3 (7.5 g, 28.2 mmol) and potassium thioacetate (3.4 g, 29.6 mmol) were heated to reflux in 100 mL of acetonitrile for 6 hours. After the reaction was completed, the solid formed was filtered off, and the solvent was distilled off from the filtrate to obtain a liquid compound. A solution of the obtained compound and sodium hydroxide (2.2 g, 55.6 mmol) in ethanol (100 mL) was heated to reflux for 6 hours, cooled to room temperature, and acidified with hydrochloric acid. Toluene was added to the reaction solution, and the solution was washed with water, the solvent was distilled off, and column purification was performed to obtain intermediate 4 as a liquid. <Synthesis Example 5> Synthesis of intermediate 5

[0305] [ka]

[0306] Hydroxybenzenethiol (10.0g, 79.2mmol), iodomethane (10.7g, 75.2mmol) and potassium carbonate (13.4g, 96.9mmol) were heated under reflux in 150mL of acetonitrile for 6 hours. After the reaction was completed, toluene was added, and the mixture was washed with water, the solvent was removed, and the mixture was purified by column chromatography to obtain intermediate 5 as a liquid. <Synthesis Example 6> Synthesis of intermediate 6

[0307] [ka]

[0308] Hydroxybenzenethiol (15.0g, 118.8mmol), bromohexane (18.63g, 112.8mmol) and potassium carbonate (24.6g, 178.2mmol) were heated under reflux in 150mL of acetonitrile for 6 hours. After the reaction was completed, toluene was added, and the mixture was washed with water, the solvent was distilled off, and purified using a column to obtain intermediate 6 as a liquid. <Synthesis Example 7> Synthesis of intermediate 7

[0309] [ka]

[0310] Hydroxybenzenethiol (10.0 g, 79.2 mmol), bromooctane (14.6 g, 75.6 mmol) and potassium carbonate (13.4 g, 96.9 mmol) were heated under reflux in 150 mL of acetonitrile for 6 hours. After the reaction was completed, toluene was added, and the mixture was washed with water, the solvent was distilled off, and purified using a column to obtain intermediate 7 as a liquid. <Synthesis Example 8> Synthesis of intermediate 8

[0311] [ka]

[0312] Hydroxybenzenethiol (10.0 g, 79.2 mmol), intermediate 3 (20.2 g, 75.6 mmol), and potassium carbonate (13.4 g, 96.9 mmol) were heated under reflux in 150 mL of acetonitrile for 6 hours. After the reaction was completed, toluene was added, and the mixture was washed with water, the solvent was distilled off, and purified using a column to obtain intermediate 8 as a liquid. <Synthesis Example 9> Synthesis of Compound 1

[0313] [ka]

[0314] 2-(2-Hydroxy-5-methylphenyl)benzotriazole (10.0 g, 44.4 mmol), intermediate 1 (11.6 g, 48.8 mmol) and potassium carbonate (12.3 g, 88.8 mmol) were heated under reflux in 100 mL of acetonitrile for 6 hours. After the reaction was completed, toluene was added, and the mixture was washed with water, the solvent was removed, and purified using a column to obtain the following intermediate 9 in liquid form.

[0315] [ka]

[0316] A solution of intermediate 9 (5.0 g, 13.1 mmol) and sodium hydroxide (1.0 g, 26.1 mmol) in ethanol (100 mL) was heated under reflux for 6 hours, then cooled to room temperature and acidified with hydrochloric acid. Toluene was added to the reaction solution, which was then washed with water, the solvent was removed, and column purification was performed to obtain compound 1 in liquid form. FT-IR(KBr):2550cm -1 :SH stretching vibration 1464, 1403cm -1 : Triazole ring stretching vibration 1073cm -1 :-O-CH2 antisymmetric stretching vibration 1 H-NMR (CDCl3400MHz): δ 1.24 (m, 5H, O-(CH2)2C H 2C H 2(CH2)2-S H ), 1.43 (m, 2H, O-(CH2)4C H 2CH2-SH), 1.63 (m, 2H, O-CH2C H 2(CH2)4-SH), 2.34 (m, 5H, O-(CH2)5C H 2-SH, -Ph-C H 3-O-), 3.99 (tri, 2H, OC H C H ) 13 C-NMR (CDCl3400MHz): δ20.0 (C arom - C H3), 24.4 (O-(CH2)5 C H2-SH), 25.4 (O-(CH2)2 C H2(CH2)3-SH), 27.8 (O-(CH2)3 C H2(CH2)2-SH), 28.8 (O-CH2 C H2(CH2)4-SH), 33.8 (O-(CH2)4 C H2CH2-SH), 69.6 (O- CH2(CH2)5-SH), 117.6, 127.7, 129.6, 131.5 ( C H arom ), 114.5, 147.5 ( C arom ), 130.5 ( C arom -CH3), 151.0 ( C arom O-) <Synthesis Example 10> Synthesis of Compound 2

[0317] [ka]

[0318] Compound 2 was synthesized using intermediate 2 (14.3 g, 48.8 mmol) in the same manner as in the synthesis of compound 1. The physical properties are shown below. FT-IR(KBr):2559cm -1 :SH stretching vibration 1465, 1403cm -1 : Triazole ring stretching vibration 1073cm -1 :-O-CH2 antisymmetric stretching vibration 1 H-NMR (CDCl3400MHz): δ 1.18 (m, 10H, O-(CH2)3(C H 2)5(CH2)2-SH) , 1.32 (m, 3H, O- (CH2)2C H 2(CH2)7-S H ), 1.60 (m, 4H, O-CH2C H 2(CH2)6C H 2CH2SH), 2.37 (s, 3H, -Ph-C H 3-O-), 2.50 (quin, 2H, O-(CH2)9C H 2SH), 4.00 (tri, 2H, OC H C H ) 1313C-NMR (CDCl3 400 MHz): δ 20.0 (C arom - C H3), 24.6 (O-(CH2)9 C H2-SH), 25.7 (O-(CH2)2 C H2(CH2)7-SH), 28.3 (O-(CH2)3 C H2(CH2)6-SH), 28.9 (O-(CH2)4 C H2(CH2)5-SH), 29.0 (O-(CH2)5 C H2(CH2)4-SH), 29.1 (O-(CH2)6 C H2(CH2)3-SH), 29.2 (O-(CH2)7 C H2(CH2)2-SH), 29.4 (O-(CH2)8 C H2CH2-SH), 34.0 (O-CH2 C H2(CH2)8-SH), 69.6 (O- C H2(CH2)9-SH), 117.6, 127.7, 129.6, 131.5( C H arom ), 114.5, 147.5 ( C arom ), 130.5 ( C arom -CH3), 151.0 ( C arom O-) <Synthesis Example 11> Synthesis of Compound 3

[0319]

Chemical Structure

[0320] After adding concentrated hydrochloric acid (11 ml, 0.13 mol) to an aqueous solution (100 mL) of nitroaniline (2.64 g, 19.1 mmol), an aqueous solution (15 mL) of sodium nitrite (2.64 g, 19.1 mmol) was added dropwise for 30 minutes under ice cooling, and the mixture was allowed to react for 30 minutes to obtain an intermediate diazonium salt. Next, the diazonium salt aqueous solution was added dropwise to an aqueous solution (150 mL) of intermediate 7 (5.0 g, 20.1 mmol) and sodium hydroxide (0.96 g, 23.9 mmol) under ice cooling over 1 hour, and the mixture was allowed to react for 1 hour. After the reaction was completed, the mixture was acidified with hydrochloric acid, toluene was added and the mixture was washed with water, and the solvent was removed and recrystallized to obtain the following intermediate 10.

[0321] [ka]

[0322] Intermediate 10 (4.50 g, 9.7 mmol), 1.2% hydrazine aqueous solution (50 ml), and sodium hydroxide (1.73 g, 34.13 mmol) were reacted in toluene (100 mL) under heating and reflux for 12 hours. After cooling to room temperature, the mixture was washed with water and the solvent was distilled off to obtain a liquid intermediate. The intermediate, concentrated sulfuric acid (0.78 mL), and zinc (3.04 g, 46.5 mmol) were reacted in toluene (100 mL) under heating and reflux for 12 hours, followed by washing with water, distillation of the solvent, and column purification to obtain compound 3 as a liquid. FT-IR(KBr):3270cm -1 :OH stretching vibration 1437, 1411cm -1 : Triazole ring stretching vibration 660cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 0.83 (t, 3H, C H 3(CH2)7-S) , 1.27 (m, 10H, CH3(C H 2)5(CH2)2-S), 1.54 (quin, 2H, CH3(CH2)5C H 2CH2-S), 2.79 (t, 2H, CH3(CH2)6C H2-S), 6.40 (s, 1H, Ph-O H ), 6.70 (d, 1H), 6.91 (s, 1H), 7.46 (m, 2H) , 7.51 (d, 1H), 7.98 (m, 2H) (insg.7arom. C H ) 13 C-NMR (CDCl3400MHz): δ 13.0 ( C H3(CH2)7-S), 21.6 (CH3 C H2(CH2)6-S), 28.0 (CH3CH2( C H2)4(CH2)2-S), 30.7 (CH3(CH2)5 C H2CH2-S), 32.0(CH3(CH2)5CH2 C H2-S), 111.6, 113.6, 117.3, 126.1, 126.9, 135.4 ( C H arom ), 131.3( C arom -S), 143.5 ( C arom ), 156.4 ( C arom OH) <Synthesis Example 12> Synthesis of Compound 4

[0323] [ka]

[0324] Compound 4 was synthesized using intermediate 8 (5.7 g, 20.1 mmol) in the same manner as in the synthesis of compound 3. The physical properties are shown below. FT-IR(KBr):3059cm -1 OH stretching vibration 1437, 1399cm -1 : Triazole ring stretching vibration 669cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 0.87 (t, 3H, C H 3(CH2)7-S), 1.25 (m, 10H, CH3(CH 2)5(CH2)2-S), 1.53 (quin, 2H, CH3(CH2)5C H 2CH2-S), 1.86 (quin, 2H, S-CH2C H 2CH2-S-Ph), 2.43 (t, 2H, CH3(CH2)6C H 2-S), 2.54 (t, 2H, SC H 2CH2CH2-S-Ph), 2.96 (t, 2H, S-CH2CH2C H 2-S-Ph), 5.95 (s, 1H, Ph-O H ),6.74 (d, 1H), 6.97 (s, 1H), 7.44 (m, 2H), 7.57 (d, 1H), 7.98 (m, 2H) (insg.7arom. C H ) 13 C-NMR (CDCl3400MHz):δ14.1( C H3(CH2)7-S), 22.6(CH3 C H2(CH2)6-S), 28.2 (CH3(CH2)2 C H2(CH2)4-S), 28.9 (CH3(CH2)5 C H2CH2-S), 29.2(CH3(CH2)3 C H2 C H2(CH2)2-S), 29.6 (CH3(CH2)6 C H2-S), 30.9 (S- C H2 C H2CH2-S), 31.8 (CH3CH2 C H2(CH2)5-S), 32.1(S-CH2CH2 C H2-S),112.9, 114.8, 118.4, 128.0, 135.7( C arom H), 127.0( C arom -N), 144.6( C arom ), 134.1( C arom -S), 156.9 ( C arom -OH) <Synthesis Example 13> Synthesis of Compound 6

[0325] [ka]

[0326] 2-(2-Hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole (60.0g, 0.190mol), butanethiol (34.3g, 0.380mol), potassium carbonate (57.8g, 0.418mol) and potassium iodide (2.21g, 0.013mol) were reacted in 150g of DMF at 125°C for 12 hours. After the reaction was completed, the pH was adjusted, and then the mixture was filtered, washed with MeOH and water, and recrystallized to obtain compound 6. FT-IR(KBr):3000cm -1 :OH stretching vibration 1445, 1392cm -1 : Triazole ring stretching vibration 661cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 0.96 (t, 3H, C H 3(CH2)3-S) , 1.49 (m, 11H, -Ph-OH-CH3-C(C H 3) 3, CH3C H 2CH2CH2-S), 1.75 (quin, 2H, CH3CH2C H 2CH2-S), 2.38 (s, 3H, -Ph-OH-C H 3-C(CH3)3) , 3.03 (t, 2H, CH3CH2CH2C H 2-S), 7.16 (s, 1H), 7.37 (d, 1H), 7.70 (s, 1H), 7.81 (d, 1H), 8.05 (d, 1H), (insg.5arom. CH), 11.61 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 C-NMR (CDCl3400MHz): δ 13.7 ( CH3(CH2)3-S), 20.9 (-Ph-OH- C H3-C(CH3)3), 22.1 (CH3 C H2CH2CH2-S), 29.5 (-Ph-OH-CH3-C( C H3)3), 30.8 (-Ph-OH-CH3- C (CH3)3), 32.8 (CH3CH2 C H2CH2-S), 35.4 (CH3CH2CH2 C H2-S), 113.6, 117.5, 119.3, 128.7, 129.3 ( C H arom ), 125.4, 141.2, 143.4 ( C arom ), 128.3 ( C arom -CH3), 138.0( C arom -S), 139.1( C arom -C(CH3)3), 146.7( C arom -OH) <Synthesis Example 14> Synthesis of Compound 7

[0327] [ka]

[0328] 2-(2-Hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole (50.0g, 0.158mol), hexanethiol (37.4g, 0.316mol), potassium carbonate (48.1g, 0.348mol) and potassium iodide (1.8g, 0.011mol) were reacted in 125g of DMF at 125°C for 12 hours. After the reaction was completed, the pH was adjusted, and then the mixture was filtered, washed with MeOH and water, and recrystallized to obtain compound 7. FT-IR(KBr):2956cm -1 :OH stretching vibration 1445, 1392cm -1 : Triazole ring stretching vibration 662cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 0.89 (t, 3H, C H 3(CH2)5-S) , 1.33 (m, 4H, CH3(C H 2)2(CH2)3-S), 1.49 (m, 11H, -Ph-OH-CH3-C(C H 3)3, CH3(CH2)2C H 2(CH2)2-S), 1.73 (quin, 2H, CH3(CH2)3C H 2CH2-S), 2.38 (s, 3H, -Ph-OH-C H 3-C(CH3)3), 3.02 (t, 2H, CH3(CH2)3CH2C H 2-S), 7.16 (s, 1H), 7.36 (d, 1H), 7.69 (s, 1H), 7.78 (d, 1H), 8.04 (s, 1H), (insg.5arom. C H ), 11.62 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 C-NMR (CDCl3400MHz): δ 14.0 ( C H3(CH2)5-S), 20.9 (-Ph-OH- C H3-C(CH3)3), 22.6 (CH3 C H2(CH2)3CH2-S), 28.7 (CH3CH2( C H2)2CH2CH2-S), 29.5 (-Ph-OH-CH3-C( C H3)3), 31.8 (-Ph-OH-CH3- C (CH3)3) , 33.8 (CH3(CH2)3 C H2CH2-S), 35.4 (CH3(CH2)3CH2 C H2-S), 113.6, 117.5, 119.3, 128.7, 129.2 ( C H arom ), 125.4, 141.2, 143.4 ( C arom ), 128.3 ( C arom-CH3), 138.0( C arom -S), 139.1( C arom -C(CH3)3), 146.7( C arom -OH) <Synthesis Example 15> Synthesis of Compound 8

[0329] [ka]

[0330] 2-(2-Hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole (5.00g, 15.8mmol), octanethiol (7.63g, 52.1mmol), potassium carbonate (7.20g, 52.1mmol) and potassium iodide (0.18g, 1.1mmol) were reacted in 50mL of DMF at 150°C for 20 hours. After the reaction was completed, toluene was added, the mixture was washed with water, the solvent was distilled off, and the mixture was purified by column chromatography to obtain compound 8. FT-IR(KBr):3125cm -1 :OH stretching vibration 1438, 1391cm -1 : Triazole ring stretching vibration 661cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 0.88 (t, 3H, C H 3(CH2)7-S) , 1.27 (m, 8H, CH3(C H 2)4(CH2)3-S), 1.49 (m, 11H, -Ph-OH-CH3-C(C H 3)3, CH3(CH2)4C H 2(CH2)2-S), 1.75 (quin, 2H, CH3(CH2)5C H 2CH2-S), 2.38 (s, 3H, -Ph-OH-C H 3-C(CH3)3) , 3.03 (t, 2H, CH3(CH2)5CH2C H2-S), 7.16 (s, 1H), 7.37 (d, 1H), 7.70 (s, 1H), 7.81 (d, 1H), 8.05 (s, 1H), (insg.5arom. C H ), 11.61 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 C-NMR (CDCl3400MHz): δ 14.0 ( C H3(CH2)7-S), 20.0 (-Ph-OH- C H3-C(CH3)3), 22.6 (-Ph-OH-CH3- C (CH3)3), 28.7 (CH3( C H2)5CH2CH2-S), 31.9 (-Ph-OH-CH3-C( C H3)3), 33.2 (CH3(CH2)5 C H2CH2-S), 35.4 (CH3(CH2)5CH2 C H2-S), 113.6, 117.5, 119.3, 128.7, 129.3 ( C H arom ), 141.2, 143.4 ( C arom ), 125.4( C arom -N), 128.3 (C arom - C H3), 138.0( C arom -S), 139.1( C arom -C(CH3)3), 146.7( C arom -OH) <Synthesis Example 16> Synthesis of Compound 9

[0331] 2-(2-ヒドロキシ-3-tert-ブチル-5-メチルフェニル)

change

[0332] -5-Chlorobenzotriazole (50.0 g, 0.158 mol), decanol (55.2 g, 0.317 mol), potassium carbonate (48.1 g, 0.348 mol) and potassium iodide (1.8 g, 0.011 mol) were reacted in 125 g of DMF at 125° C. for 12 hours. After the reaction was completed, the pH was adjusted, and then the mixture was filtered, washed with MeOH and water, and recrystallized to obtain compound 9. FT-IR(KBr):2958cm -1 :OH stretching vibration 1448, 1392cm -1 : Triazole ring stretching vibration 641cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 0.89 (t, 3H, C H 3(CH2)9-S) , 1.26 (m, 12H, CH3(C H 2)6(CH2)3-S), 1.49 (m, 11H, -Ph-OH-CH3-C(C H 3)3, CH3(CH2)6C H 2(CH2)2-S), 1.74 (quin, 2H, CH3(CH2)7C H 2CH2-S), 2.38 (s, 3H, -Ph-OH-C H 3-C(CH3)3) , 3.03 (t, 2H, CH3(CH2)7CH2C H 2-S), 7.16 (s, 1H), 7.36 (d, 1H), 7.69 (s, 1H), 7.78 (d, 1H), 8.05 (s, 1H), (insg. H ), 11.62 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 C-NMR (CDCl3400MHz): δ 14.0 ( C H3(CH2)9-S), 20.9 (-Ph-OH- C H3-C(CH3)3), 22.7 (CH3 C H2(CH2)7CH2-S), 28.7 ~ 29.5 (CH3CH2( CH2)6CH2CH2-S), 29.6 (-Ph-OH-CH3-C( C H3)3), 31.9 (-Ph-OH-CH3- C (CH3)3), 33.1 (CH3(CH2)7 C H2CH2-S), 35.4 (CH3(CH2)7CH2 C H2-S), 113.6, 117.5, 119.3, 128.7, 129.3 ( C H arom ), 125.4, 141.2, 143.4 ( C arom ), 128.3 ( C arom -CH3), 138.0( C arom -S), 139.1( C arom -C(CH3)3), 146.7( C arom -OH) <Synthesis Example 17> Synthesis of Compound 10

[0333] [ka]

[0334] Compound 10 was synthesized using dodecanethiol (10.5 g, 52.1 mmol) instead of octanethiol in the same synthesis method as compound 8. The physical properties are shown below. FT-IR(KBr):3009cm -1 :OH stretching vibration 1441, 1390cm -1 : Triazole ring stretching vibration 662cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 0.88 (t, 3H, C H 3 (CH2) 11 -S), 1.25 (m, 16H, CH3(C H 2)8(CH2)3-S), 1.49 (m, 11H, -Ph-OH-CH3-C(C H 3)3, CH3(CH2)8CH 2(CH2)2-S), 1.74 (quin, 2H, CH3(CH2)9C H 2CH2-S), 2.38 (s, 3H, -Ph-OH-C H 3-C(CH3)3), 3.03 (t, 2H, CH3(CH2) 10 C H 2-S), 7.16 (s, 1H), 7.37 (d, 1H), 7.70 (s, 1H), 7.81 (d, 1H), 8.05 (s, 1H) (insg.5arom. C H ), 11.61 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 C-NMR (CDCl3 400MHz): δ 14.0 ( C H3(CH2) 11 -S), 20.9 (-Ph-OH- C H3-C(CH3)3), 22.7 (-Ph-OH-CH3- C (CH3)3), 28.7 ~ 29.7 (CH3( C H2)9CH2CH2-S), 31.9 (-Ph-OH-CH3-C( C H3)3), 33.2 (CH3(CH2)9 C H2CH2-S), 35.4 (CH3(CH2)9CH2 C H2-S), 113.5, 117.5, 119.3, 128.6, 129.3 ( C H arom ), 141.2, 143.4 ( C arom ), 125.4( C arom -N), 128.3 (C arom - C H3), 138.0( C arom -S), 139.1( C arom -C(CH3)3), 146.7( C arom -OH) <Synthesis Example 18> Synthesis of Compound 11

[0335] [ka]

[0336] Compound 11 was synthesized using the same synthesis method as for compound 8, except that octadecanethiol (14.9 g, 52.1 mmol) was used instead of octanethiol. The physical properties are shown below. FT-IR(KBr):3059cm -1 :OH stretching vibration 1445, 1391cm -1 : Triazole ring stretching vibration 664cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 0.88 (t, 3H, C H 3 (CH2) 17 -S), 1.25 (m, 30H, CH3(C H 2) 15 (CH2)2-S), 1.49 (s, 9H, -Ph-OH-CH3-C(CH 3 )3, 1.74 (quin, 2H, CH3(CH2) 15 C H 2CH2-S), 2.38 (s, 3H, -Ph-OH-C H 3-C(CH3)3) , 3.03 (t, 2H, CH3(CH2) 15 CH2C H 2-S), 7.16 (s, 1H), 7.37 (d, 1H), 7.70 (s, 1H), 7.81 (d, 1H), 8.05 (s, 1H) (insg.5arom. H ), 11.61 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 C-NMR (CDCl3400MHz): δ 13.1( C H3(CH2) 17 -S), 19.9(-Ph-OH- C H3-C(CH3)3), 21.6 (-Ph-OH-CH3- C (CH3)3), 28.5(CH3(C H2) 16 CH2-S), 30.6(C arom -(-Ph-OH-CH3-C( C H3)3), 34.4 (CH3(CH2) 16 C H2-S), 115.5, 117.6, 118.2, 127.2, 128.0 ( C H arom ), 141.9, 142.9 ( C arom ), 124.2( C arom -N), 128.1 (C arom - C H3), 132.3 ( C arom -S), 140.0 ( C arom -C(CH3)3), 145.6 ( C arom -OH) <Synthesis Example 19> Synthesis of Compound 12

[0337] [ka]

[0338] 2-(3,5-Di-tert-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole (25.0 g, 69.85 mmol), butanethiol (20.43 g, 139.71 mmol), potassium carbonate (21.23 g, 153.68 mmol), and potassium iodide (2.21 g, 4.82 mmol) were reacted in 150 g of DMF at 125° C. for 12 hours. After the reaction was completed, the pH was adjusted, the mixture was filtered and washed with MeOH, and then the pH was adjusted again, washed with water, and recrystallized to obtain compound 12. FT-IR(KBr):2953cm -1 :OH stretching vibration 1439, 1392cm -1 : Triazole ring stretching vibration 667cm -1 :CS stretching vibration 1H-NMR (CDCl3400MHz): δ 0.88 (t, 3H, C H 3(CH2)7-S) , 1.27 (m, 8H, CH3(C H 2)4(CH2)3-S), 1.39 (s, 9H, -Ph-OH-C(C H 3)3-C(CH3)3) , 1.51 (m, 11H, -Ph-OH-C(CH3)3-C(C H 3)3, CH3(CH2)2C H 2(CH2)2-S), 1.75 (quin, 2H, CH3(CH2)5C H 2CH2-S), 3.03 (t, 2H, CH3(CH2)5CH2C H 2-S), 7.37 (d, 1H), 7.40 (s, 1H), 7.71 (s, 1H), 7.82 (d, 1H), 8.24 (d, 1H), (insg.5arom. C H ), 11.66 (s, 1H, -Ph-O H - C(CH3)3-C(CH3)3) 13 C-NMR (CDCl3400MHz):δ 14.1 ( C H3(CH2)7-S), 22.6(CH3 C H2(CH2)6-S), 28.7 ~ 29.2(CH3CH2( C H2)4CH2CH2-S), 29.6 (-Ph-OH-C(CH3)3-C( C H3)3), 31.5 (-Ph-OH-C( C H3)3-C(CH3)3) , 31.8 (CH3CH2(CH2)4 C H2CH2-S) , 33.2 (-Ph-OH- C (CH3)3-C(CH3)3), 34.6 (CH3(CH2)4CH2 C H2-S), 35.7 (-Ph-OH-C(CH3)3- C (CH3)3), 113.6, 116.0, 117.6, 129.2, 143.4 ( C H arom ), 125.0, 141.2, 143.4 ( Carom ), 137.9( C arom -S), 125.2, 138.6( C arom -C(CH3)3), 146.6( C arom -OH) <Synthesis Example 20> Synthesis of Compound 13

[0339] [ka]

[0340] 2-(3,5-di-tert-butyl-2-hydroxyphenyl)-5-chlorobenzotriazole (25.0 g, 69.85 mmol), dodecanethiol (28.28 g, 139.72 mmol), potassium carbonate (21.24 g, 153.68 mmol) and potassium iodide (0.81 g, 4.88 mmol) were reacted in 62.5 g of DMF at 125° C. for 12 hours. After the reaction was completed, the pH was adjusted, the mixture was filtered and washed with MeOH, and then the pH was adjusted again, washed with water, and recrystallized to obtain compound 13. FT-IR(KBr):2962cm -1 :OH stretching vibration 1434, 1389cm -1 :Triazole ring stretching vibration 668cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 0.87(t, 3H, C H 3 (CH2) 11 -S), 1.26 (m, 16H, CH3(C H 2)8(CH2)3-S), 1.39 (s, 9H, -Ph-OH-C(C H 3)3-C(CH3)3) , 1.51 (m, 11H, -Ph-OH-C(CH3)3-C(C H 3)3, CH3(CH2)8C H 2(CH2)2-S), 1.74 (quin, 2H, CH3(CH2)9C H2CH2-S), 3.03 (t, 2H, CH3(CH2)9CH2C H 2-S), 7.35 (d, 1H), 7.41 (s, 1H), 7.71 (s, 1H), 7.82 (d, 1H), 8.24 (d, 1H), (insg.5arom. C H ), 11.67 (s, 1H, -Ph-O H - C(CH3)3-C(CH3)3) 13 C-NMR (CDCl3 400MHz): δ 14.1 ( C H3(CH2) 11 -S), 22.7 (CH3 C H2(CH2) 10 -S), 28.7 ~ 29.7 (CH3CH2( C H2)8CH2CH2-S), 29.6 (-Ph-OH-C(CH3)3-C( C H3)3), 31.5 (-Ph-OH-C( C H3)3-C(CH3)3), 31.9 (CH3(CH2)9 C H2CH2-S), 33.2 (-Ph-OH- C (CH3)3-C(CH3)3), 34.6 (CH3(CH2)9CH2 C H2-S), 35.7 (-Ph-OH-C(CH3)3- C (CH3)3), 113.6, 116.0, 117.6, 129.2, 143.4 ( C H arom ), 125.0, 141.2, 143.4 ( C arom ), 137.9( C arom -S), 125.2, 138.6( C arom -C(CH3)3), 146.6( C arom -OH) <Synthesis Example 21> Synthesis of Compound 14

[0341]

Chemical Structure

[0342] Using intermediate 4 (11.5 g, 52.1 mmol), compound 14 was synthesized in the same synthetic method as compound 7. The physical property values are shown below. FT-IR (KBr): 3057 cm -1 : O-H stretching vibration 1437, 1391 cm -1 : Triazole ring stretching vibration 664 cm -1 : C-S stretching vibration 1 1H-NMR (CDCl3 400 MHz): δ 0.81 (t, 3H, C H 3(CH2)7-S), 1.20 (m, 8H, CH3(C H 2)4(CH2)3-S), 1.30 (m, 2H, CH3(CH2)4C H 2(CH2)2-S), 1.49 (s, 9H, -Ph-OH-CH3-C(C H 3)3), 1.54 (quin, 2H, CH3(CH2)4CH2C H 2CH2-S), 1.91(quin, 2H, S-CH2C H 2CH2-S-Ph), 2.38(s, 3H, -Ph-OH-C H 3-C(CH3)3), 2.48 (t, 2H, CH3(CH2)4CH2CH2C H 2-S), 2.68 (t, 2H, S-C H 2CH2CH2-S-Ph), 3.17 (t, 2H, S-CH2CH2C H 2-S-Ph), 7.16 (s, 1H), 7.37 (d, 1H), 7.70 (s, 1H), 7.81 (d, 1H), 8.05 (d, 1H), (insg.5arom. C H ), 11.61 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 13C-NMR (CDCl3 400 MHz): δ14.0( C H3(CH2)7-S), 20.1(-Ph-OH- C H3-C(CH3)3), 22.6(-Ph-OH-CH3-C (CH3)3), 28.4(CH3 C H2(CH2)6-S), 28.9(CH3(CH2)5 C H2CH2-S), 29.2(CH3(CH2)3 C H2 C H2(CH2)2-S), 29.6(CH3(CH2)6 C H2-S), 30.9 (S- C H2CH2CH2-S), 31.8 (CH3CH2 C H2(CH2)5-S), 31.9(-Ph-OH-CH3-C( C H3)3), 32.2(S-CH2 C H2CH2-S), 35.4(S-CH2CH2 C H2-S),114.4, 117.6, 119.3, 128.7, 129.4 ( C H arom ), 141.3, 143.3 ( C arom ), 125.4( C arom -N), 128.3 (C arom - C H3), 137.1( C arom -S), 139.1( C arom -C(CH3)3), 146.7( C arom -OH) <Synthesis Example 22> Synthesis of Compound 15

[0343]

change

[0344] 2-(2-Hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole (36.3 g, 0.115 mol), sec-butyl mercaptan (20.8 g, 0.231 mol), potassium carbonate (35.0 g, 0.253 mol) and potassium iodide (1.3 g, 0.008 mol) were reacted in 100 g of DMF at 125° C. for 12 hours. After the reaction was completed, the pH was adjusted, filtered, washed with MeOH and water, and recrystallized to obtain compound 15. FT-IR(KBr):2961cm -1 :OH stretching vibration 1448, 1391cm -1 : Triazole ring stretching vibration 665cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 1.06 (t, 3H, C H 3CH2CH(CH3)-S), 1.37 (d, 3H, CH3CH2CH(C H 3)-S), 1.49 (S, 9H, -Ph-OH-CH3-C(C H 3)3), 1.61 (m, 2H, CH3C H 2CH(CH3)-S), 2.38 (s, 3H, -Ph-OH-C H 3-C(CH3)3), 3.32 (m, 1H, CH3CH2C H (CH3)-S), 7.17 (s, 1H), 7.42 (d, 1H), 7.80 (s, 1H), 7.84 (d, 1H), 8.06 (d, 1H), (Insg. H ), 11.62 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 C-NMR (CDCl3400MHz): δ 11.5 ( C H3CH2CH(CH3)-S), 20.3 (CH3CH2CH( C H3)-S), 20.9 (-Ph-OH- C H3-C(CH3)3), 29.4 (CH3 CH2CH(CH3)-S), 29.5 (-Ph-OH-CH3-C( C H3)3), 35.4 (-Ph-OH-CH3- C (CH3)3), 44.6 (CH3CH2 C H(CH3)-S), 117.3, 117.5, 119.3, 128.3, 128.8 ( C H arom ), 141.5, 143.2 ( C arom ), 125.4 ( C arom -N), 131.2 ( C arom -CH3), 136.4 ( C arom -S), 139.1 ( C arom -C(CH3)3), 146.7 ( C arom -OH) <Synthesis Example 23> Synthesis of Compound 16

[0345] [ka]

[0346] 2-(2-Hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole (32.3 g, 0.102 mol), cyclohexanethiol (23.8 g, 0.205 mol), potassium carbonate (31.1 g, 0.225 mol) and potassium iodide (1.2 g, 0.007 mol) were reacted in 100 g of DMF at 125° C. for 12 hours. After the reaction was completed, the pH was adjusted, filtered, washed with MeOH and water, and recrystallized to obtain compound 16. FT-IR(KBr):2930cm -1 :OH stretching vibration 1450, 1391cm -1 : Triazole ring stretching vibration 667cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 1.40 (m, 4H, CH2(CH 2)2(CH2)2CH-S), 1.49 (S, 9H, -Ph-OH-CH3-C(C H 3)3), 1.54 (m, 2H, C H 2(CH2)2(CH2)2CH-S), 1.83 (m, 2H, CH2(CH2)2CH2C H 2CH-S), 2.06 (m, 2H, CH2(CH2)2C H 2CH2CH-S), 2.38 (s, 3H, -Ph-OH-C H 3-C(CH3)3), 3.29 (m, 1H, CH2CH2CH2C H -S), 7.17 (s, 1H), 7.43 (d, 1H), 7.80 (s, 1H), 7.84 (d, 1H), 8.06 (d, 1H), (insg.5arom. C H ), 11.62 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 C-NMR (CDCl3400MHz): δ 20.9 (-Ph-OH- C H3-C(CH3)3), 25.7 (CH2( C H2)2(CH2)2CH-S), 26.0 ( C H2(CH2)2(CH2)2CH-S), 29.5 (-Ph-OH-CH3-C( C H3)3), 33.1 (CH2(CH2)2( C H2)2CH-S), 35.4 (-Ph-OH-CH3- C (CH3)3), 46.3 (CH2(CH2)2(CH2)2 C H-S), 117.2, 117.5, 119.3, 128.3, 128.8 ( C H arom ), 141.5, 143.2 ( C arom ), 125.4 ( C arom -N), 131.2 ( C arom -CH3), 136.1 ( C arom-S), 139.1 ( C arom -C(CH3)3), 146.7 ( C arom -OH) <Synthesis Example 24> Synthesis of Compound 17

[0347] [ka]

[0348] 2-(2-Hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole (50.0 g, 0.158 mol), allyl mercaptan (23.5 g, 0.317 mol), potassium carbonate (48.1 g, 0.348 mol) and potassium iodide (1.8 g, 0.011 mol) were reacted in 125 g of DMF at 125° C. for 12 hours. After the reaction was completed, the pH was adjusted, filtered, washed with MeOH and water, and recrystallized to obtain compound 17. FT-IR(KBr):3092cm -1 OH stretching vibration 2999cm -1 :=CH stretching vibration 1449, 1390cm -1 : Triazole ring stretching vibration 664cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 1.49 (S, 9H, -Ph-OH-CH3-C(C H 3)3), 1.55 (m, 2H, CH2=CHC H 2-S), 2.38 (s, 3H, -Ph-OH-C H 3-C(CH3)3), 3.38 (m, 1H, C H 2=CHCH2-S), 3.78 (m, 1H, C H 2=CHCH2-S), 4.23 (m, 1H, CH2=C H C), 7.16 (s, 1H), 7.31 (d, 1H), 7.71 (s, 1H), 7.73 (d, 1H), 8.05 (d, 1H), (insg. H), 11.66 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 C-NMR (CDCl3400MHz): δ 21.0 (-Ph-OH- C H3-C(CH3)3), 22.5 ( C H2=CHCH2-S), 29.6 (-Ph-OH-CH3-C( C H3)3), 35.4 (-Ph-OH-CH3- C (CH3)3), 41.8 (CH2= C HCH2-S), 46.3 (CH2=CH C H2-S), 116.7, 119.3, 123.3, 128.2, 128.6 ( C H arom ), 140.8, 141.7 ( C arom ), 125.4 ( C arom -N), 124.1 ( C arom -CH3), 140.7 ( C arom -S), 139.0 ( C arom -C(CH3)3), 146.6 ( C arom -OH) <Synthesis Example 25> Synthesis of Compound 18

[0349] [ka]

[0350] 2-(2-hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole (25.0 g, 79.2 mmol), p-toluenethiol (19.7 g, 158.3 mmol), potassium carbonate (24.1, 174.2 mmol), potassium iodide (0.92 g, 5.54 mmol), and 62.5 g of DMF were reacted at 125° C. for 12 hours. After the reaction was completed, the pH was adjusted, and the mixture was filtered, washed with MeOH, washed with water, and recrystallized to obtain compound 18. FT-IR (KBr): 3000 cm -1 : O-H stretching vibration at 1444, 1389 cm -1 : Triazole ring stretching vibration at 667 cm -1 : C-S stretching vibration 1 H-NMR (CDCl3 400 MHz): δ1.48 (s, 9H, -Ph-OH-CH3-C(C H 3)3), 2.37 (s, 3H, -Ph-OH-C H 3-C(CH3)3), 2.40 (s, 3H, C H 3-Ph-S-), 7.16 (s, 1H), 7.23 (s, 2H), 7.32 (d, 1H), 7.43 (s, 2H), 7.56 (s, 1H), 7.81 (d, 1H), 8.02 (d, 1H), (insg.9arom. C H ), 11.56 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 C-NMR (CDCl3 400 MHz): δ20.9 (-Ph-OH- C H3-C(CH3)3), 21.2 ( C H3-Ph-S-), 29.5 (-Ph-OH-CH3-C( C H3)3), 35.4 (-Ph-OH-CH3- C (CH3)3), 115.3, 117.8, 119.3, 128.7, 129.3 130.5, 133.7(CH arom ), 125.4, 141.2, 143.4 (C arom ), 128.3 ( C arom -CH3), 138.9( C arom -S), 138.7(S - C arom ), 139.1( C arom -C(CH3)3), 146.7( C arom -OH) <Synthesis Example 26> Synthesis of Compound 19

[0351] [ka]

[0352] 2-(2-Hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole (20.0 g, 63.3 mmol), benzyl mercaptan (15.7 g, 126.6 mmol), potassium carbonate (19.3 g, 139.4 mmol) and potassium iodide (0.74 g, 4.5 mmol) were reacted in 50.0 g of DMF at 125° C. for 9 hours. After the reaction was completed, the pH was adjusted, and the mixture was filtered, washed with MeOH and water, and recrystallized to obtain compound 19. FT-IR(KBr):2960cm -1 :OH stretching vibration 1441, 1392cm -1 : Triazole ring stretching vibration 664cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ1.49 (s, 9H, -Ph-OH-CH3-C(C H 3) 3), 2.38 (s, 3H, -Ph-OH-C H 3-C(CH3)3) , 4.24 (s, 2H, Ph-C H 2-S-) , 7.16 (s, 1H), 7.26~7.38 (m, 6H), 7.72 (s, 1H), 7.80 (d, 1H), 8.04 (d, 1H), (insg.10 arom CH), 11.58 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 C-NMR (CDCl3400MHz): δ20.9 (-Ph-OH- C H3-C(CH3)3), 29.5 (-Ph-OH-CH3-C( C H3)3), 35.4 (-Ph-OH-CH3- C (CH3)3), 38.6 (Ph- CH2-S-), 115.4, 117.6, 119.3, 128.7, 128.8, 128.8, 129.7, 137.0( C H arom ), 125.4, 141.4, 143.4 ( C arom ), 128.3 ( C arom -CH3), 136.5( C arom CH2-S-), 138.7(S - C arom ), 139.1( C arom -C(CH3)3), 146.7( C arom -OH) <Synthesis Example 27> Synthesis of Compound 20

[0353] [ka]

[0354] 2-(2-Hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole (50.5 g, 0.160 mol), 2-mercaptoethanol (25.0 g, 0.320 mol), potassium carbonate (48.6 g, 0.352 mol) and potassium iodide (1.9 g, 0.011 mol) were reacted in 125 g of DMF at 125° C. for 12 hours. After the reaction was completed, the pH was adjusted, filtered, washed with MeOH and water, and recrystallized to obtain compound 20. FT-IR(KBr):3350cm -1 :OH stretching vibration 1437, 1392cm -1 : Triazole ring stretching vibration 666cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 1.49 (S, 9H, -Ph-OH-CH3-C(C H 3) 3), 2.38 (s, 3H, -Ph-OH-C H 3-C(CH3)3), 2.79 (t, 2H, HOCH2CH 2-S), 3.25 (t, 2H, HOC H 2CH2-S), 7.17 (s, 1H), 7.41 (d, 1H), 7.83 (s, 1H), 7.84 (d, 1H), 8.05 (d, 1H), (insg.5arom. C H ), 11.56 (s, 1H, -Ph-O H -CH3-C(CH3)3) 13 C-NMR (CDCl3400MHz): δ 20.9 (-Ph-OH- C H3-C(CH3)3), 29.5 (-Ph-OH-CH3-C( C H3)3), 35.4 (-Ph-OH-CH3- C (CH3)3), 36.8 (HOCH2 C H2-S), 60.3 (HO C H2CH2-S), 115.8, 118.0, 119.3, 128.4, 129.7 ( C H arom ), 141.5, 143.2 ( C arom ), 125.3 ( C arom -N), 128.9 ( C arom -CH3), 135.7 ( C arom -S), 139.2 ( C arom -C(CH3)3), 146.7 ( C arom -OH) <Synthesis Example 28> Synthesis of Compound 21

[0355]

change

[0356] 2-(2-Hydroxy-3-tert-butyl-5-methylphenyl)-5-chlorobenzotriazole (10.0 g, 31.7 mmol), hexanedithiol (4.76 g, 31.7 mmol), potassium carbonate (8.75 g, 63.3 mmol), and potassium iodide (0.37 g, 2.2 mmol) were reacted in 50 mL of DMF at 130° C. for 12 hours. After the reaction was completed, toluene was added, the mixture was washed with water, the solvent was distilled off, and recrystallization was performed to obtain compound 21. FT-IR(KBr):3009cm -1 :OH stretching vibration 1431, 1391cm -1 : Triazole ring stretching vibration 656cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ1.49 (s, 18H, (-Ph-OH-CH3-C(C H 3)3)2), 1.55 (m, 4H, -S-CH2CH2C H 2C H 2CH2CH2-S-), 1.77 (m, 4H, -S-CH2C H 2CH2CH2C H 2CH2-S-), 2.38(s, 6H, (-Ph-OH-C H 3-C(CH3)3)2) , 3.04 (t, 4H, -SC H 2CH2CH2CH2CH2C H C H ), 11.60 (s, 2H, -Ph-OH-CH3-C(CH3)3) 13 C-NMR (CDCl3400MHz): δ20.9 (-Ph-OH- C H3-C(CH3)3)2, 28.4 (-Ph-OH-CH3- C (CH3)3)2, 28.6 (-S-CH2CH2 C H2 CH2CH2CH2-S-), 29.5 (-Ph-OH-CH3-C( C H3)3)2, 33.1 (-S-CH2 C H2CH2CH2 C H2CH2-S-), 35.4 (-S- C H2CH2CH2CH2CH2 C H2-S-), 113.7, 117.6, 119.3, 128.3, 129.3 ( C H arom ), 141.2, 143.4 ( C arom ), 125.4( C arom -N), 128.3 ( C arom -CH3), 137.7( C arom -S), 139.1( C arom -C(CH3)3), 146.7( C arom -OH) <Synthesis Example 29> Synthesis of Compound 22

[0357] [ka]

[0358] 2,4-Dihydroxybenzophenone (8.6g, 40mmol), 1,4-diazabicyclo[2.2.2]octane (9.0g, 80mmol) and dimethylthiocarbamoyl chloride (6.18g, 50mmol) were reacted in 100mL of DMF at 80°C for 12 hours. After the reaction was completed, toluene was added, and the mixture was washed with water, the solvent was distilled off, and purified using a column to obtain the following intermediate 11.

[0359] [ka]

[0360] Intermediate 11 (5.0 g, 16.6 mmol) was reacted in 10 mL of sulfolane at 240° C. for 40 minutes. After the reaction was completed, toluene was added, and the mixture was washed with water, the solvent was distilled off, and purified using a column to obtain Intermediate 12 below.

[0361] [ka]

[0362] Intermediate 12 (3.46 g, 11.4 mmol) and potassium hydroxide (3.22 g, 57.4 mmol) were reacted in 100 mL of ethanol under heating and reflux for 6 hours. After the reaction was completed, the mixture was acidified with hydrochloric acid, toluene was added, and the mixture was washed with water, the solvent was removed, and the mixture was purified by column chromatography to obtain compound 22. FT-IR(KBr):3055cm -1 :OH stretching vibration 2559cm -1 :SH stretching vibration 1624cm -1 :C=O stretching vibration 1 H-NMR (CDCl3400MHz): δ 3.65 (s, 1H, -Ph-OH-S H ), 6.68 (d, 1H), 6.93 (s, 1H), 7.44 (d, 1H), 7.51 (m, 2H) , 7.58 (m, 1H) , 7.65 (d, 2H) (insg.8arom. C H ), 12.28 (s, 1H, -Ph-O H -SH) 13 C-NMR (CDCl3400MHz):δ 115.4, 117.5, 127.4, 128.0 ( C H arom ), δ 130.9, 132.9 ( C arom ), δ 142.26 ( C arom SH), δ 162.5 ( C arom -OH), δ 199.6 ( C (=O)) <Synthesis Example 30> Synthesis of Compound 23

[0363] [ka]

[0364] 4-Chloro-4'-hydroxybenzophenone (5.44g, 23.4mmol), octanethiol (6.84g, 46.8mmol), and potassium carbonate (13.7g, 99.2mmol) were reacted in 2mL of N-methylpyrrolidone at 200°C for 4 hours. After the reaction was completed, toluene was added, and the mixture was washed with water, the solvent was distilled off, and purified using a column to obtain compound 23. FT-IR(KBr):3266cm -1 :OH stretching vibration 1630cm -1 :C=O stretching vibration 646cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 0.88 (t, 3H, C H 3(CH2)7-S), 1.28 (m, 8H, CH3(C H 2)4(CH2)3-S), 1.45 (m, 2H, CH3(CH2)4C H 2CH2CH2-S), 1.71 (quin, 2H, CH3(CH2)5C H 2CH2-S), 3.00 (t, 2H, CH3(CH2)5CH2C H 2-S), 6.22 (s, 1H, -S-Ph-C=O-Ph-O H ), 6.92(d, 2H), 7.31(d, 2H), 7.68(d, 2H), 7.74(d, 2H) (insg.8arom. C H ) 13 C-NMR (CDCl3400MHz): δ14.1( C H3(CH2)7-S), 22.6(CH3 C H2(CH2)5-S), 28.8 (CH3(CH2)4 C H2(CH2)2-S), 28.9 (CH3(CH2)3 CH2(CH2)3-S), 29.1(CH3CH2 C H2(CH2)4-S), 31.8(CH3 C H2CH2(CH2)4-S), 32.2 (CH3(CH2)6 C H2-S), 115.3, 126.3, 130.5, 132.8( C H arom ), 134.4 ( C arom ), 143.9 ( C arom S-), 160.3( C arom -OH), 195.4 (Ph- C (=O)-Ph) <Synthesis Example 31> Synthesis of Compound 24

[0365] [ka]

[0366] Intermediate 3 (1.20 g, 4.7 mmol), compound 22 (2.00 g, 8.6 mmol) and potassium carbonate (2.40 g, 17.2 mmol) were reacted in 30 mL of acetonitrile under reflux for 6 hours. After the reaction was completed, toluene was added, and the mixture was washed with water, the solvent was removed, and the mixture was purified using a column to obtain compound 24. FT-IR(KBr):3059cm -1 :OH telescopic vibration 1615cm -1 :C=O stretching vibration 669cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz):δ 0.88 (t, 3H, C H 3(CH2)7-S), 1.28 (m, 4H, CH3(C H 2)4(CH2)3-S), 1.37 (m, 2H, CH3(CH2)4C H 2(CH2)2-S), 1.58 (m, 2H, CH3(CH2)5C H 2CH2-S), 2.00 (quin, 2H, S-CH2C H2CH2-S-Ph), 2.51 (t, 2H, CH3(CH2)5CH2C H 2-S), 2.67 (t, 2H, S-C H 2CH2CH2-S-Ph), 3.12 (t, 2H, S-CH2CH2C H 2-S-Ph), 6.71 (d, 1H), 6.90 (s, 1H), 7.44 (d, 1H), 7.51 (m, 2H), 7.58 (m, 1H), 7.65 (d, 2H) (insg.8arom. C H ), 12.37 (s, 1H, -Ph-O H -S-) 13 C-NMR (CDCl3 400MHz): δ14.1( C H3(CH2)7-S), 22.7(CH3 C H2(CH2)6-S), 28.3 (CH3(CH2)3 C H2(CH2)3-S), 28.9 (CH3(CH2)5 C H2CH2-S), 29.2(CH3(CH2)3 C H2 C H2(CH2)2-S), 29.7 (CH3(CH2)6 C H2-S), 30.1 (S- C H2CH2CH2-S), 30.9 (S-CH2 C H2CH2-S), 31.8 (CH3CH2 C H2(CH2)5-S), 32.2(S-CH2CH2 C H2-S), 114.1, 116.0, 116.7, 128.4, 129.0, 131.8, 133.5 ( C H arom ), 130.9, 132.9 ( C arom ), 138.0 ( C arom S-), 163.7 ( C arom -OH), 200.5 (Ph- C (=O)-Ph) <Synthesis Example 32> Synthesis of Compound 25

[0367] [ka]

[0368] 4-Chloro-4'-hydroxybenzophenone (1.68g, 7.2mmol), intermediate 4 (2.54g, 11.5mmol), and potassium carbonate (1.60g, 11.5mmol) were reacted in 2mL of N-methylpyrrolidone at 200°C for 4 hours. After the reaction was completed, toluene was added, and the mixture was washed with water, the solvent was distilled off, and purified using a column to obtain compound 25 as a liquid containing 90% or more. FT-IR(KBr):3266cm -1 :OH stretching vibration 1630cm -1 :C=O stretching vibration 646cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 0.80 (t, 3H, C H 3(CH2)7-S), 1.20 (m, 8H, CH3(C H 2)4(CH2)3-S), 1.30 (m, 2H, CH3(CH2)4C H 2CH2CH2-S), 1.50 (quin, 2H, CH3(CH2)5C H 2CH2-S), 1.91 (quin, 2H, S-CH2C H 2CH2-S-Ph),2.43 (t, 2H, CH3(CH2)6C H 2-S), 2.60 (t, 2H, SC H 2CH2CH2-S-Ph), 3.00 (t, 2H, S-CH2CH2C H 2-S-Ph), 5.93 (s, 1H, -Ph-C=O-Ph-O H ), 6.83(d, 2H), 7.30(d, 2H), 7.68(d, 2H), 7.63(d, 2H) (insg.8arom. C H ) 13 C-NMR (CDCl3400MHz): δ14.1( C H3(CH2)7-S), 22.6(CH3C H2(CH2)6-S), 28.5 (CH3(CH2)2 C H2(CH2)3-S), 28.9 (CH3(CH2)5 C H2CH2-S), 29.2(CH3(CH2)3 C H2 C H2(CH2)2-S), 29.7 (CH3(CH2)6 C H2-S), 30.9 (S- C H2CH2CH2-S), 31.0 (S-CH2 C H2CH2-S), 31.8 (CH3CH2 C H2(CH2)5-S), 32.4(S-CH2CH2 C H2-S), 114.4, 125.5, 128.6, 129.6( C H arom ), 131.9, 133.2 ( C arom ), 142.3 ( C arom S-), 159.8( C arom -OH), 194.5 (Ph- C (=O)-Ph) <Synthesis Example 33> Synthesis of Compound 26

[0369] [ka]

[0370] Salicylic acid (8.8g, 63.9mmol) and thionyl chloride (22.8g, 191.6mmol) were reacted at 25°C for 3 hours, and then unreacted thionyl chloride was distilled off under reduced pressure to obtain intermediate salicylic acid chloride (9.8g, 62.6mmol). The obtained salicylic acid chloride (2.50g, 16.0mmol), intermediate 6 (3.86g, 18.35mmol) and potassium carbonate (2.20g, 15.91mmol) were reacted in 100mL of toluene under heating and reflux for 12 hours. After the reaction was completed, toluene was added, the mixture was washed with water, the solvent was distilled off, and the mixture was purified by column to obtain compound 26 as a liquid. FT-IR(KBr):3229cm-1 : O-H stretching vibration at 1694 cm -1 : C=O-O stretching vibration at 593 cm -1 : C-S stretching vibration 1 H-NMR (CDCl3 400 MHz): δ 0.88 (t, 3H, C H 3(CH2)5-S), 1.29 (m, 4H, CH3(C H 2)2(CH2)3-S), 1.45 (m, 2H, CH3(CH2)2C H 2(CH2)2-S), 1.67 (quin, 2H, CH3(CH2)3C H 2CH2-S), 2.96 (t, 2H, CH3(CH2)3CH2C H 2-S), 6.99 (m, 2H), 7.05 (d, 1H), 7.14 (s, 1H), 7.22 (d, 1H), 7.25 (t, 1H), 7.56 (t, 1H), 8.01 (d, 1H), (insg. 8 arom. C H ), 10.47 (s, 1H, -Ph-O H ) 13 C-NMR (CDCl3 400 MHz): δ 14.0 ( C H3(CH2)5-S), 22.5 (CH3 C H2(CH2)4-S), 28.9 (CH3CH2( C H2)2CH2CH2-S), 31.3 (CH3(CH2)3 C H2CH2-S), 33.3 (CH3(CH2)4 C H2-S), 111.8, 118.6, 119.5, 121.2, 129.2, 130.3 ( C H arom ), 117.9 ( C arom -C(=O)-O-), 139.5( C arom -S), 150.4 (-(O=)C-O- C arom ) , δ 162.3( C arom -OH) , δ 168.7 ( C(=O)-) <Synthesis Example 34> Synthesis of Compound 27

[0371]

Chem.

[0372] Compound 27 was synthesized in the same manner as Compound 26 using 3,5 - di - tert - butyl - 4 - hydroxybenzoic acid (16.0 g, 63.9 mmol). FT - IR (KBr): 3622 cm -1 : O - H stretching vibration 1732 cm -1 : C = O - O stretching vibration 639 cm -1 : C - S stretching vibration 1 1H - NMR (CDCl3 400 MHz): δ 0.88 (t, 3H, C H 3(CH2)5 - S), 1.29 (m, 4H, CH3(C H 2)2(CH2)3 - S), 1.43(m, 2H, CH3(CH2)2C H 2(CH2)2 - S), 1.49 (s, 18H, - Ph - OH - (C(C H 3)3)2), 1.67 (quin, 2H, CH3(CH2)3C H 2CH2 - S), 2.93 (t, 2H, CH3(CH2)3CH2C H 2 - S), 5.77(s, 1H, - Ph - O H -(C(CH3)3)2), 6.98 (d, 1H), 7.13 (s, 1H), 7.17 (d, 1H), 7.30 (t, 1H), 8.04 (s, 2H) (insg.6arom. C H ) 13 13C - NMR (CDCl3 400 MHz): δ 14.0 ( C H3(CH2)6 - S), 22.5 (- Ph - OH -( C (CH3)3)2)), 28.5(CH3 C H2(CH2)4 - S), 28.9 (CH3(CH2)2 CH2(CH2)2-S), 30.2 (-Ph-OH-(C( C H3)3)2)), 31.3 (CH3CH2 C H2(CH2)2CH2-S), 33.4 (CH3(CH2)3 C H2CH2-S), 34.1 (CH3(CH2)4 C H2-S), 119.1, 120.3, 121.8, 127.8, 129.4 ( C H arom ), 125.7( C arom -C(=O)-O-), 136.0(- C arom - (C(CH3)3)2), 138.8( C arom -S), 151.5(-(O=)CO- C arom ), δ 158.8( C arom -OH), δ 165.5 ( C (=O)-) <Synthesis Example 35> Synthesis of Compound 28

[0373] [ka]

[0374] 2-Chloro-4,6-diphenyl-1,3,5-triazine (1.92 g, 7.14 mmol) and aluminum chloride (2.37 g, 17.85 mmol) were reacted in 50 mL of O-xylene at 25° C. for 30 minutes, and then intermediate 5 (2.00 g, 14.25 mmol) was added and reacted at 80° C. for 8 hours. After the reaction was completed, toluene was added, the mixture was washed with water, the solvent was removed, column purification was performed, and recrystallization was performed to obtain compound 28. FT-IR(KBr):3064cm -1 :OH stretching vibration 1568, 845cm -1 : Triazine ring stretching vibration 602cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 2.41 (s, 3H, Ph-SCH 3), 6.71 (m, 2H), 7.47 (m, 6H), 8.47 (m, 5H) (insg.13arom. C H ), 13.28 (s, 1H,Ph-O H ) 13 C-NMR (CDCl3400MHz): δ 14.7 (Ph-S C H3), 114.1 ((HO-)C arom C arom C(-N)=N), 113.2, 128.8, 129.0, 129.8, 133.0( C H arom ), 148.2 ( C arom -SCH3), 162.4 ( C arom -OH), 171.4 (N-(C arom )- C =N). <Synthesis Example 36> Synthesis of Compound 29

[0375] [ka]

[0376] Cyanuric acid chloride (1.92 g, 7.14 mmol) and intermediate 6 (6.75 g, 32.13 mmol) were dissolved in 50 mL of 1,2-dichloroethane by heating, then cooled with ice, and aluminum chloride (0.95 g, 7.14 mmol) was added over 30 minutes, followed by reaction at 70° C. for 54 hours. After the reaction was completed, toluene was added, the mixture was washed with water, the solvent was removed, column purification was performed, and recrystallization was performed to synthesize compound 29. FT-IR(KBr):3064cm -1 :OH stretching vibration 1568, 846cm -1 : Triazine ring stretching vibration 602cm -1 :CS stretching vibration 1 H-NMR (CDCl3400MHz): δ 0.92 (t, 3H, C H3(CH2)5-S), 1.34 (m, 4H, CH3(C H 2)2(CH2)3-S), 1.47 (quin, 2H, CH3(CH2)2C H 2(CH2)2-S), 1.75 (quin, 2H, CH3(CH2)3C H 2CH2-S), 3.02 (t, 2H, CH3(CH2)3CH2C H 2-S), 6.89 (d, 2H), 7.62 (m, 6H), 8.58 (d, 1H), 8.63 (m, 4H) (insg.13arom. C H ), 13.43 (s, 1H, Ph-O H ) 13 C-NMR (CDCl3400MHz): δ 14.0 ( C H3(CH2)5-S), 22.5(CH3 C H2(CH2)4-S), 28.6 (CH3CH2 C H2(CH2)3-S), 28.7 (CH3(CH2)2CH2(CH2)2-S), 31.4 (CH3(CH2)3 C H2CH2-S), 31.5(CH3(CH2)4 C H2-S), 111.9 ( C arom C=N), 114.1, 117.9, 128.5 ( C H arom ), 149.6 ( C arom -S), 162.7 ( C arom -OH), 168.4 (C arom - C =N). <Synthesis Example 37> Synthesis of Compound 30

[0377]

change

[0378] Intermediate 7 (7.66 g, 32.13 mmol) was synthesized using the same synthesis method as compound 29 and compound 30. FT-IR (KBr): 2951 cm -1 : O-H stretching vibration 1570, 843 cm -1 : Triazine ring stretching vibration 606 cm -1 : C-S stretching vibration 1 H-NMR (CDCl3 400 MHz): δ 0.90 (t, 3H, C H 3(CH2)7-S), 1.32 (m, 8H, CH3(C H 2)4(CH2)3-S), 1.47 (quin, 2H, CH3(CH2)4C H 2(CH2)2-S), 1.72 (quin, 2H, CH3(CH2)5C H 2CH2-S), 2.92 (t, 2H, CH3(CH2)6C H 2-S), 6.70 (d, 2H), 7.72 (d, 1H), (insg.13arom. C H ), 12.99 (s, 1H, Ph-O H ) 13 C-NMR (CDCl3 400 MHz): δ 14.1 ( C H3(CH2)7-S), 22.7 (CH3 C H2(CH2)6-S), 28.6 (CH3CH2 C H2(CH2)5-S), 29.2 (CH3(CH2)2( C H2)3(CH2)2-S), 31.5 (CH3(CH2)5 C H2CH2-S), 31.9 (CH3(CH2)6 C H2-S), 111.8 ( C arom C=N), 113.9, 117.7, 128.4 ( C H arom ), 149.6 ( C arom -S), 162.7 ( C arom -OH), 168.2 (C arom - C =N) <Synthesis Example 38> Synthesis of Compound 31

[0379]

Chem.

[0380] Using intermediate 6 (2.0 g, 8.38 mmol), compound 31 was synthesized in the same synthetic method as compound 28. The physical property values are shown below. FT-IR (KBr): 33064 cm -1 : O-H stretching vibration 1568, 846 cm -1 : Triazine ring stretching vibration 602 cm -1 : C-S stretching vibration 1 1H-NMR (CDCl3 400 MHz): δ 0.90 (t, 3H, C H 3(CH2)5-S), 1.34 (m, 2H, CH3(C H 2)2(CH2)3-S), 1.47 (quin, 2H, CH3(CH2)2C H 2(CH2)2-S), 1.75 (quin, 2H, CH3(CH2)3C H 2CH2-S), 3.03 (t, 2H, CH3(CH2)3CH2C H 2-S), 6.89 (d, 2H), 7.62 (m, 6H), 8.58 (d, 1H), 8.63 (m, 4H) (insg. 13 arom. C H ), 13.43 (s, 1H, Ph-O H ) 13 13C-NMR (CDCl3 400 MHz): δ 14.0 ( C H3(CH2)5-S), 22.5(CH3 C H2(CH2)4-S), 28.7 (CH3CH2 C H2(CH2)3-S), 28.8 (CH3(CH2)2 C H2(CH2)2-S), 31.4 (CH3(CH2)3 C H2CH2-S), 31.8(CH3(CH2)4 C H2-S), 114.3 ((HO-)C C aromC(-N)=N),117.9, 129.0, 129.9, 133.0 ( C H arom ), 135.3 ( C arom -C=N), 147.4 ( C arom -S), 162.3 ( C arom -OH), 171.4 (C arom - C =N). Compound 5 was manufactured by Sigma-Aldrich, compound 32 was manufactured by BASF, compound 33 was manufactured by Tokyo Chemical Industry Co., Ltd., compound 34 was manufactured by Wako Pure Chemical Industries, Ltd., compound 35 was manufactured by Sigma-Aldrich, and compound 36 was manufactured by Tokyo Chemical Industry Co., Ltd.

[0381] The evaluation results of the melting points, film appearances, and refractive indices of the compounds of the Examples and Comparative Examples are shown in Tables 1 to 8, and the ultraviolet-visible transmission spectra of the compounds of the Examples are shown in FIGS. 1. Compound Evaluation (1) Melting point The melting points of the compounds of Examples and Comparative Examples 2 to 4 were measured by visual observation (liquid or solid) at room temperature (25°C) or by using a micro melting point measuring device (MP-3 manufactured by Yanako) or a differential scanning calorimeter (DSC6220 manufactured by SII) (Tables 1 to 7).

[0382] Benzotriazole compounds containing a thiol group have the functional group -(CH2) n The melting point was 35°C or less when the number of carbon atoms in -SH was 1 to 10 (compounds 1 and 2). 1a ~R 5a The compounds containing a thioether group (compounds 3 and 4), benzophenone (compounds 24 and 25), and salicylate compounds (compounds 26 and 27) have a functional group -(CH2) n -S- or -S-(CH2) n -S- or -S-(CH2) nWhen the maximum number of carbon atoms in CH3 is 8 or less, the melting point is 35°C or less, and the compound is liquid at room temperature. It was confirmed that there is a correlation between the number of carbon atoms and the melting point, regardless of the skeleton of benzotriazole, benzophenone, or salicylate. 6a ~R 9a The benzotriazole compounds (compounds 6-14) that have a thioether group consisting of a linear aliphatic saturated hydrocarbon group on the -(CH2) functional group n -S- or -S-(CH2) n -S- or -S-(CH2) n Compounds with a maximum carbon number of 18 or less in CH3 (compounds 6 to 14) have melting points of 91°C or less, but there is no clear correlation between the carbon number and the melting point, making it difficult to lower the melting point.

[0383] In addition, compared with compound 32 having an ether group (-O-), compound 3 having a thioether group (-S-) had a lower melting point and was liquid at room temperature. Furthermore, compound 14 having two thioether groups had a lower melting point than compounds 6 to 13 having one thioether group, confirming the tendency for the introduction of a thioether to lower the melting point.

[0384] On the other hand, the introduction of a sulfur-containing group into triazine-based compound 28 increased its melting point, suggesting that it has excellent heat resistance. (2) Refractive index The refractive indexes of compounds 1, 2, 3, 4, 5, 25, 26, and 27, which have melting points of 25° C. or less, were measured at 20° C., and those of compounds 14 (46° C.) and 24 (34° C.), which have relatively low melting points, were measured by heating using an Abbe refractometer (NAR-2T manufactured by Atago Co., Ltd.). For Comparative Examples 2, 3, and 4 (compounds 32, 33, and 34), the manufacturer's catalog values ​​and the like are listed.

[0385] Among the benzotriazole-based compounds, compounds 1 to 4 and 14 have higher refractive indexes than compounds 5 and 32, among the benzophenone-based compounds, compounds 24 and 25 have higher refractive indexes than compound 33, and among the salicylate-based compounds, compounds 26 and 27 have higher refractive indexes than compound 34, confirming the effect of increasing the refractive index by introducing a sulfur-containing group. (3)5% weight loss temperature Compounds 6 to 21, 23, 24, 27, 29, 30, 31, 33, 34, 35, and 36 were measured using a simultaneous differential thermal / thermogravimetric analyzer (TG / DTA6200, manufactured by SII) at a heating rate of 10°C / min and a measurement range of 25°C to 550°C, and the temperature at which the weight change (TG) decreased by 5 wt% was read.

[0386] Benzotriazole compounds and bis-forms (compound 21) having thioether groups composed of saturated and unsaturated hydrocarbon groups (compounds 6 to 17), aromatic groups (compounds 18 and 19), and oxygen-containing hydrocarbon groups (compound 20) have improved heat resistance by introducing a thioether group (suppressing the decrease in the UV absorption ability of resin parts, the ability to increase the refractive index, and the transparency of transparent resins due to thermal decomposition of the UV absorber). Their 5% weight loss decomposition temperatures were 252°C or higher, which was higher than that of 2-(2-hydroxy-3-t-butyl-5-methylphenyl)-chlorobenzotriazole (compound 36, 5% weight loss decomposition temperature: 230°C), which does not have a sulfur-containing group and is generally used as a long-wavelength absorbing UV absorber, or compound 5 (5% weight loss decomposition temperature: 249°C). Similarly, for benzophenone and salicylate compounds, benzophenone compounds 23 (5% weight loss decomposition temperature: 279°C) and 24 (5% weight loss decomposition temperature: 260°C) had improved heat resistance at 5% weight loss decomposition temperatures of 260°C or higher compared to compound 33 (5% weight loss decomposition temperature: 249°C) which does not have a thioether group, and salicylate compound 27 (5% weight loss decomposition temperature: 264°C) had improved heat resistance at 5% weight loss decomposition temperatures of 260°C or higher compared to compound 34 (5% weight loss decomposition temperature: 249°C) which does not have a thioether group. In other words, the 5% weight loss decomposition temperatures of compounds 6 to 21, 23, 24, and 27 are higher than the softening temperatures of most common resins, which are 100 to 250°C ("Easy-to-Understand Plastics", edited by the Japan Plastics Industry Federation, published by Nihon Jitsugyo Publishing). Generally, these compounds are applicable to thermosetting resins and thermoplastic resins that require a molding temperature of 100 to 200°C, as well as to thermoplastic resins that require a molding temperature higher than 200 to 250°C, making it possible to suppress the decrease in the ultraviolet absorption ability and high refractive index of resin parts, and the decrease in the transparency of transparent resin parts.

[0387] In addition, for triazine-based compounds, compared with compound 35 (5% weight loss temperature: 319°C) which does not have a thioether group, compound 29 (5% weight loss temperature: 369°C), compound 30 (5% weight loss temperature: 372°C), and compound 31 (5% weight loss temperature: 336°C) which have a thioether group introduced therein also show that the 5% weight loss temperature is increased by the introduction of a thioether group, and the heat resistance (suppression of the decrease in the ultraviolet absorption ability of the resin component, the ability to increase the refractive index, and the transparency of the transparent resin due to the thermal decomposition of the ultraviolet absorber) is improved, and it has been confirmed that these compounds are applicable to thermoplastic resins which require a molding processing temperature higher than 200 to 250°C. (4) Ultraviolet absorption Compounds 1-5, 8, 10, 11, 14, 22-35 were diluted with chloroform to 5 μM and placed in a 10 mm quartz cell, and their absorption spectra were measured using a UV-Vis spectrophotometer (JASCO Corporation, V-550) (Figures 1-2, 6-8). Compounds 6-21 and 36 were similarly measured with chloroform at 100 μM (Figures 3-5).

[0388] From the absorption spectrum (100μM) of compounds 8, 10, 11, 14, 21, 36, the intersection point of the absorption spectrum on the long wavelength side of the absorption peak at 350-390nm and the baseline (the line where the absorption spectrum slope at 430-500nm is 0) was set as the peak end (example: Example 47 in Fig. 3), and the absolute value of the slope on the long wavelength side of the absorption peak in the wavelength region of 350-390nm was calculated by the following formula (Table 9). Similarly, the absolute value of the slope on the long wavelength side of the absorption peak in the wavelength region of 350-390nm was calculated from the absorption spectrum of compounds 6, 7, 9, 12, 13, 15-20 and is shown in Tables 2 and 4. |Slope of the long wavelength side of the absorption peak in the wavelength range of 350 to 390 nm|=|(Absorbance of the peak end - Absorbance of the absorption peak in the wavelength range of 350 to 390 nm) / (Absorption wavelength of the peak end - Wavelength of the absorption peak in the wavelength range of 350 to 390 nm)| The absolute value of the slope of compounds 6 to 21 was all 0.030 or more, which was larger than that of compound 36, which does not have a thioether group (absolute value of the slope on the long-wavelength side of the absorption peak in the wavelength region of 350 to 390 nm: 0.0219), and the peak was sharper, suggesting that the compounds have a yellowing suppression effect on films and resin parts, especially transparent resin parts.

[0389] In addition, for compound 21, the molar extinction coefficient was large, and when measured at 100 μM, the absorbance exceeded the measurement range, so as shown in Table 10, the absorption peak was measured at concentrations of 10, 25, and 50 μM, and the absolute value of the slope on the long wavelength side of the absorption peak in the wavelength region of 350 to 390 nm and the concentration of the ultraviolet absorber were graphed. As shown in Figure 9, there is a linear linear relationship, and the absolute value of the slope of 100 μM of compound 21 was calculated from the graph formula (Y = 0.0006X-0.0024). As a result, the slope of 100 μM of compound 21 was 0.0576, which was larger than the other compounds, and it was considered that the yellow suppression effect on films, resin members, especially transparent resin members, was high.

[0390] From the absorption spectra of compounds 6 to 21 and 36, the absorption peaks in the wavelength range of 350 to 390 nm (maximum absorption wavelength: λ max ), the absorbance was read, and the molar absorption coefficient of that peak (maximum molar absorption coefficient: ε max ) was calculated using the following formula (Table 11). Molar extinction coefficient: ε max (L / (mol cm) = A: absorbance / [c: molar concentration (mol / L) × l: cell path length (cm)] As a result, compounds 6 to 21, which contain thioether, have a higher molar absorption coefficient of 17,000 or more than compound 36, and it was shown that even a small amount of compound 21 can efficiently absorb ultraviolet light. In particular, the bis-compound 21 has a higher molar absorption coefficient than compounds 6 to 20, and its effect is considered to be even greater.

[0391] It was confirmed that all of the compounds of the present invention have an absorption band in the ultraviolet wavelength region, and function as an ultraviolet absorber when added to a film or resin.

[0392] The benzotriazole compounds 6 to 21 of the present invention, in which the thioether group i-2 is introduced into the benzotriazole group, have been confirmed to have ultraviolet absorbing ability that can absorb ultraviolet rays in the longer wavelength region of 360 to 400 nm even in the UV-A region (320 to 400 nm) without cutting (yellowing) 420 to 500 nm (visible region), which is not found in 2-(2-hydroxy-3-t-butyl-5-methylphenyl)-chlorobenzotriazole (Comparative Example 10, Compound 36, Figures 3 to 5) that is conventionally used as a long-wavelength absorbing ultraviolet absorbing agent. In addition, the compounds 1, 2, 3, and 4, in which the thioether group i-2 is introduced into the phenyl group on the nitrogen of the benzotriazole compound, have the absorption peak tops shifted significantly to the short wavelength region (270 to 290 nm) in contrast to the compound 32 of Comparative Example 9. In other words, in the benzotriazole compounds, the UV absorption peak region can be adjusted by the position of the thioether group.

[0393] Due to this property, in Examples 71 to 77 (Figures 10 to 16), it was confirmed that adding a small amount of the additive of the present invention to a plastic lens efficiently absorbs harmful light with wavelengths of around 400 to 420 nm while suppressing absorption of wavelengths of around 420 nm or more, thereby suppressing yellowing of the plastic lens.

[0394] It was also confirmed that the introduction of the iv-2 substituent into triazine-based compounds 28 to 31 shifted the absorption peak top to the long wavelength region larger than that of Comparative Example 13 (compound 35), and could absorb ultraviolet rays in the long wavelength region of about 360 to 400 nm without cutting visible light (450 to 500 nm). Furthermore, it was confirmed that triazine-based compounds 28 and 31 have an absorption peak top in the short wavelength ultraviolet region (260 to 280 nm) in addition to an absorption peak top in the longer wavelength region (about 360 to 400 nm), and can absorb ultraviolet rays in a wide region. 2. Film evaluation The compatibility (transparency) of the compound of the present invention with films and resin members and the effect of increasing the refractive index were confirmed by the following method (Tables 1 to 8). (Preparation of acrylic film) The following three types of films having different thicknesses were prepared by adding the compounds of Examples 1 to 14, 22 to 29, and Comparative Examples 2 and 3.

[0395] Samples with a film thickness of 50 to 300 nm were prepared by uniformly mixing 0.1 g of each of the compounds of Examples 1 to 14, 22 to 27 and Comparative Examples 2 to 3, 0.1 g of acrylic resin (manufactured by Mitsubishi Rayon Co., Ltd.), and 12 g of chloroform, spin-coating approximately 1 mL of the mixture onto a glass substrate at 1500 rpm for 20 seconds, and then removing the solvent in an oven at 45°C for 2 hours.

[0396] Samples with a film thickness of 301 to 1500 nm were prepared by uniformly mixing 0.1 g of each of the compounds of Examples 1 to 14, 22 to 27 and Comparative Examples 2 to 3, 0.1 g of acrylic resin, and 4 g of chloroform, spin-coating approximately 1 mL of the mixture onto a glass substrate at 1500 rpm for 20 seconds, and then removing the solvent in an oven at 45°C for 2 hours.

[0397] Samples with a thickness of 10 to 150 μm were prepared by uniformly mixing 0.1 g of the compound of Examples 1 to 14, 22 to 27 and Comparative Examples 2 to 3, 0.1 g of acrylic resin, and 4 g of chloroform, concentrating the chloroform to about 2 to 3 g, dropping this onto a slide glass, and then removing the solvent in an oven at 45° C. for 2 hours.

[0398] In Examples 28 (film thickness 50-300 nm, 301-1500 nm, 10-150 μm) and 29 (film thickness 50-300 nm, 301-1500 nm), the compound and resin were mixed in amounts of 0.03 g and 0.07 g, respectively, and the same procedure was carried out.

[0399] Also, without adding any additive, 0.1 g of acrylic resin and 4 g or 12 g of chloroform were uniformly mixed, and the same operation as above was carried out to prepare a film (Comparative Example 1). (Preparation of urethane film) 0.022 g of isocyanate (HC-210, manufactured by Nippon Polyurethane Co., Ltd.), 0.078 g of polyol (ON-H37, manufactured by Nippon Polyurethane Co., Ltd.), and 0.1 g of the compound of Examples 1, 3 to 13, 22, 24 to 27, and Comparative Example 2 were uniformly mixed with 12 g of chloroform for samples with film thicknesses of 50 to 300 nm, and 4 g of chloroform for samples with film thicknesses of 301 to 1500 nm. Approximately 1 mL of each was spin-coated onto a glass substrate at 1500 rpm for 20 seconds, followed by removing the chloroform in an oven at 45°C and then heating at 100°C for 3 hours to prepare a film.

[0400] Samples with a thickness of 10 to 150 μm were prepared by uniformly mixing 0.1 g of the compounds of Examples 4, 5, 8, and 26 and Comparative Example 2, 0.022 g of isocyanate, 0.078 g of polyol, and 4 g of chloroform, concentrating the chloroform to about 2 to 3 g, dropping this onto a slide glass, removing the solvent in an oven at 45° C. for 2 hours, and then heating at 100° C. for 3 hours.

[0401] In Example 28 (film thickness 50 to 300 nm, 301 to 1500 nm, 10 to 150 μm), the compound and resin were mixed in amounts of 0.03 g and 0.07 g (isocyanate 0.015 g, polyol 0.055 g), and the same procedure as above was carried out.

[0402] Also, without adding any additives, 0.022 g of isocyanate, 0.078 g of polyol, and 4 g or 12 g of chloroform were uniformly mixed, and the same operation as above was carried out to prepare a film (Comparative Example 1). (Preparation of thiourethane film) 0.430g of compound 6, 0.1g of Stefan Zerec UN, 0.04g of dibutyltin dichloride, and 50.8g of a mixture of 2,5-bis(isocyanatomethyl)-bicyclo[2,2,1]heptane and 2,6-bis(isocyanatomethyl)-bicyclo[2,2,1]heptane were placed in a flask and stirred at 25°C for 1 hour to completely dissolve. Then, 22.4g of pentaerythritol tetrakis(3-mercaptopropionate) and 26.8g of 1,2-bis[(2-mercaptoethyl)thio]-3-mercaptopropane were added to the mixture and mixed at 25°C for 30 minutes. In addition, compound 6 was contained in the prepared solution at 0.430% by weight relative to the total weight of the polymerizable compounds.

[0403] This mixture was degassed at 0.3 mmHg or less for 1 hour, filtered with a 5 μm PTFE filter, and poured into a mold consisting of a flat glass mold with a center thickness of 2 mm and a diameter of 80 mm and a tape. The mold was gradually heated from 25°C to 130°C, held at 130°C for 2 hours, and then cooled to room temperature. It took 18 hours from the start of the temperature increase to the cooling. After the polymerization was completed, the obtained molded body was released from the mold and annealed at 130°C for 2 hours.

[0404] In addition, a thiourethane film was obtained in the same manner as for compound 6, except that the ultraviolet absorber added was changed to 0.472 g of compound 7, 0.490 g of compound 8, 0.533 g of compound 9, 0.555 g of compound 10, 0.651 g of compound 11, 0.580 g of compound 12, and 0.600 g of compound 13, with the same molar concentrations, instead of compound 6.

[0405] The thiourethane film to which compound 13 was added became cloudy due to the precipitation of crystals, whereas the thiourethane films to which compounds 6 to 12 were added were transparent without the precipitation of crystals. (Preparation of polyethylene terephthalate film: PET) To prepare the sample containing 5 wt% additive, 0.0418 g of polyethylene terephthalate chips and 0.0022 g of compounds 1, 3, 5 to 13, 25, and 28 (Examples 6 to 13, and 30 to 35) and compounds 32, 33, and 35 (Comparative Examples 6 to 8) were kneaded at 280°C, dropped onto a slide glass substrate, quickly spread, and air-cooled to produce a film of 20 to 200 μm.

[0406] To prepare the sample containing 10 wt% additive, 0.0450 g of polyethylene terephthalate chips and 0.005 g of each of compounds 1, 3, 5 to 13, 25, and 28 (Examples 6 to 13, and 30 to 35) and compounds 32, 33, and 35 (Comparative Examples 6 to 8) were kneaded at 280°C, dropped onto a slide glass substrate, quickly spread, and air-cooled to produce a film of 20 to 200 μm.

[0407] To prepare a sample containing 20 wt% additive, 0.0352 g of polyethylene terephthalate chips and 0.0088 g of compounds 1, 3, 5, 8, 25, and 28 (Examples 30 to 35) and compounds 32, 33, and 35 (Comparative Examples 6 to 8) were kneaded at 280°C, dropped onto a slide glass substrate, quickly spread, and air-cooled to produce a film of 20 to 200 μm.

[0408] To prepare a sample containing 30 wt% additive, 0.0566 g of polyethylene terephthalate chips and 0.0244 g of compounds 1, 3, 5, 8, 25, and 28 (Examples 30 to 35) and compounds 32, 33, and 35 (Comparative Examples 6 to 8) were kneaded at 280°C, dropped onto a slide glass substrate, quickly spread, and air-cooled to produce a film of 20 to 200 μm.

[0409] Also, without adding any additives, 0.045 g of polyethylene terephthalate chips were dissolved, and the same operation as above was carried out to prepare films with a thickness of 20 to 200 μm (Comparative Examples 1 and 5). (Preparation of polystyrene film: PS) Films having a thickness of 10 to 50 μm, to which the compounds of Examples 6 to 13, 15 to 18, and 20 were added, were prepared by the following procedure.

[0410] 0.1 g of each of the compounds of Examples 6 to 13, 15 to 18, and 20, 0.1 g of polystyrene resin (Kanto Chemical), and 4 g of chloroform were uniformly mixed, and then the chloroform was concentrated to about 2 to 3 g. 50 μL of this was dropped onto a slide glass, and the solvent was then removed in an oven at 45° C. for 2 hours to prepare a sample (50 wt %).

[0411] For compounds 19 and 21, 0.0111 g of compound 19 and 21, 0.1 g of polystyrene resin (Kanto Chemical), and 2 g of chloroform were mixed (10 wt%). For the blank film of Comparative Example 1, no additives were added, and 0.1 g of polystyrene resin and 4 g of chloroform were uniformly mixed and the same operation as above was carried out to prepare the film. (Preparation of polycarbonate film: PC) Films having a thickness of 10 to 50 μm, to which the compounds of Examples 6 to 13, 15 to 18, and 20 were added, were prepared by the following procedure.

[0412] 0.0667 g of the compound of Examples 6 to 13, 15 to 18, and 20, 0.1 g of polycarbonate resin (Kanto Chemical), and 4 g of chloroform were uniformly mixed, and then the chloroform was concentrated to about 2 to 3 g. 25 μL of this was dropped onto a slide glass, and the solvent was then removed in an oven at 45° C. for 2 hours to prepare a sample (40 wt %).

[0413] Compound 19 was prepared by mixing 0.011 g of compound 19, 0.1 g of polycarbonate resin (Kanto Chemical), and 2 g of chloroform (10 wt%), while compound 21 was prepared by mixing 0.025 g of compound 21, 0.1 g of polycarbonate resin (Kanto Chemical), and 4 g of chloroform (20 wt%). The blank film of Comparative Example 1 was prepared by uniformly mixing 0.1 g of polycarbonate resin and 4 g of chloroform without adding any additives, and by carrying out the same procedure as above. (Preparation of urea resin film) Films with a thickness of 40 to 80 μm, to which the compounds of Examples 6 to 13 were added, were prepared by the following procedure. 1 mL of 37 wt% formaldehyde solution, 0.25 g of urea, and 0.16 g of ammonium acetate were dissolved to prepare a monomer solution. Next, 0.0007 g of the compounds of Examples 6 to 13 were dissolved in 0.2 mL of THF, and mixed uniformly with 0.1 mL of the monomer solution, and 0.3 mL of the solution was applied to a 1.5×1.5 cm slide glass. The slide glass was then placed in an oven, and the temperature was raised from room temperature to 150° C. over 30 minutes, and the film was then reacted at 150° C. for 5 hours to prepare a film.

[0414] A blank film for comparison was prepared by homogeneously mixing 0.1 mL of the monomer solution and 0.2 mL of THF without adding any additives, and carrying out the same procedure as above (Comparative Example 1). (Preparation of melamine resin film) Films having thicknesses of 10 to 50 μm to which the compounds of Examples 6 to 13 were added were prepared according to the following procedure.

[0415] 1g of melamine and 24.60g of water were added to 5.15g of formaldehyde solution adjusted to pH 7.5 with sodium hydroxide, and the mixture was heated to react, to prepare a hexamethylolmelamine solution. Next, 0.0057g of the compounds of Examples 6 to 13 were dissolved in 0.1mL of THF, and mixed uniformly with 0.2mL of the hexamethylolmelamine solution, and 0.3mL was applied to a 1.5×1.5cm slide glass. The slide glass was then placed in an oven, heated from room temperature to 150°C over 30 minutes, and reacted at 150°C for 5 hours to prepare the solution.

[0416] A blank film for comparison was prepared by uniformly mixing 0.2 ml of the monomer solution and 0.1 ml of THF without adding any additives, and carrying out the same procedure as above (Comparative Example 1). (Creating acrylic melamine resin film) Films having a thickness of 100 to 150 μm, to which the compounds of Examples 6 to 13 were added, were prepared according to the following procedure.

[0417] When the film was made, 0.0045 g of the compounds of Examples 6 to 13 were dissolved in 0.1 mL of THF so that the concentration of the compounds was 10 wt%, and the mixture was mixed uniformly with 0.1 mL of bake-dry type topcoat paint (baked-dry type topcoat (acrylic melamine): Acrysite UB-63 Clear, manufactured by Saito Paint Co., Ltd.), and 0.2 mL of the mixture was applied to a 1.5 x 1.5 cm slide glass. The slide glass was then placed in an oven, heated from room temperature to 150 ° C. over 30 minutes, and reacted at 150 ° C. for 2 hours to obtain an acrylic melamine resin film containing 10 wt% additive.

[0418] In addition, a blank film for comparison was prepared by adding no additives, by uniformly mixing 0.1 mL of acrylic melamine monomer and 0.1 mL of THF, and by carrying out the same procedure as above (Comparative Example 1). (1) Appearance The appearance of the film was visually observed and rated according to the following criteria. Evaluation criteria (acrylic film, urethane film, thiourethane film) ○: Transparent, no cloudiness ×: White turbidity is observed and transparency is poor. Evaluation criteria (PET film) ◎: Has the same transparency as the blank of the comparative example ○: Very slightly cloudy compared to the blank of the comparative example △: Slightly cloudy compared to the blank of the comparative example ×: Clearly cloudy compared to the blank of the comparative example Evaluation criteria (PS film) ○: Has the same transparency as the blank of the comparative example △: Slightly cloudy compared to the blank of the comparative example ×: Clearly cloudy compared to the blank of the comparative example Evaluation criteria (PC film) ○: Has the same transparency as the blank of the comparative example △: Slightly cloudy compared to the blank of the comparative example ×: Clearly cloudy compared to the blank of the comparative example Evaluation criteria (urea resin film) ○: Transparent with no crystal precipitation △: Slight crystal precipitation is observed, but the product is transparent. ×: Crystal precipitation was observed and transparency was poor. Evaluation criteria (melamine resin film) ○: Transparent with no crystal precipitation ×: Crystal precipitation was observed and transparency was poor. Evaluation criteria (acrylic melamine resin film) ○: Transparent with no crystal precipitation △: Crystal precipitation is observed in some areas and transparency is poor. ×: Crystal precipitation is observed throughout the film, and transparency is poor. The alkyl chain, melting point and sulfur-containing group of the additive combined to improve the compatibility (clarification) of the thermoplastic resin with the acrylic film.

[0419] The alkyl chains are functional groups -(CH2) in the 50-300 nm films. n -SH and -(CH2) n The number of carbon atoms in each of the CH3 groups is 9 or less (compounds 1 and 22). Compounds with thioether groups have the functional group -(CH2). n -S- or -S-(CH2) n -S- or -S-(CH2) n When the carbon number of each CH3 was 17 or less (compounds 3, 4, 6-10, 12-14, 23-29), the compound was transparent. Furthermore, in the compounds having a thioether group, the compounds having a carbon number of 8 or less were generally transparent even in the thicker film of 301 to 1500 nm (compounds 3, 4, 7, 8, 12, 14, 23-27). In other words, it was confirmed that the number of carbon atoms is important for compatibility (transparency) with the resin, and that compounds having a medium to short alkyl chain tend to have improved compatibility (transparency).

[0420] For benzotriazole, benzophenone, and salicylate compounds, in addition to the correlation with the alkyl chains mentioned above, the melting point generally correlates with the compatibility with resins, and lowering the melting point improved the compatibility (transparency). Compounds with melting points of 91°C or less (compounds 1, 3, 4, 5, 6-10, 12-14, 22-27) generally became transparent in films of 50-300 nm, despite a high addition rate of 50%. Compounds with melting points below 70°C (compounds 1, 3, 4, 5, 7, 8, 9, 14, 23-27) became transparent in thicker films of 301-1500 nm, and compounds with melting points of 35°C or less (liquid at room temperature) (compounds 1, 3, 4, 24-27) achieved transparency even in thicker films of 10-150 μm.

[0421] However, in an acrylic film having a thickness of 10 to 150 μm, compounds 3 and 4 having a sulfur-containing group and a melting point of 35° C. or less became transparent, whereas compound 5 having no sulfur-containing group became cloudy, even though its melting point was 25° C. or less.

[0422] On the other hand, compounds 6 to 10, 12, and 13, which were prepared by using 2-(2-hydroxy-3-t-butyl-5-methylphenyl)-chlorobenzotriazole (Comparative Example 10, Compound 36) as a raw material and had a sulfur-containing group introduced therein, became transparent in a urethane film having a thickness of 50 to 300 nm, whereas 2-(2-hydroxy-3-t-butyl-5-methylphenyl)-chlorobenzotriazole (Comparative Example 10, Compound 36), which does not have a sulfur-containing group, became cloudy, suggesting that the introduction of a sulfur-containing group is one of the requirements for compatibility (transparency) with resins.

[0423] Compound 33, which does not have a sulfur-containing group, has a lower melting point of 47 to 48°C compared to compound 22, which has a melting point of 91°C, and compound 23, which has a melting point of 60.5 to 69°C. However, while compounds 22 and 23 became transparent in an acrylic film with a thickness of 50 to 300 nm, compound 33 became cloudy. In other words, it was suggested that not only the melting point but also the presence of a sulfur-containing group improves the compatibility (transparency) with the resin.

[0424] Furthermore, compound 2 (carbon number 10) with thiol has a melting point of 25°C or less, and compound 11 (carbon number 18) with thioether has a melting point of 73-83°C, and although the melting points are 91°C or less, acrylic films of 50-300 nm did not become transparent. In other words, it is also important to satisfy the requirements of both melting point and carbon number, and compounds 2 and 11 have carbon numbers of 10 and 18, respectively, which are greater than the above carbon numbers (compounds with thiol groups: carbon number 9 or less, compounds with thioether groups: carbon number 17 or less), and therefore did not satisfy the carbon number condition, which is thought to be why they did not become transparent.

[0425] The same tendency was observed in urethane resins, which are thermosetting resins, and they showed good transparency due to the effects of the alkyl chain, melting point and sulfur-containing group of the additive of the present invention.

[0426] In addition, due to the effects of the alkyl chain, melting point, and sulfur-containing group, compounds 1, 3, 8, 25, and 28 of the present invention also exhibited good heat resistance to the thermoplastic resin PET resin at a heat molding temperature of 280°C (5w% weight loss temperature: compound 8; 295°C, compound 5; 249°C), and showed high compatibility and good transparency compared to compounds 5, 32, 33, and 35 under conditions of high concentration and high film thickness of 20 to 200 μm (Table 8).

[0427] R in Formula I 7a , R 8a Regarding compounds 6 to 13 having formula i-2, in the evaluation (Tables 2 and 3) of compatibility (transparency) with each resin (acrylic (50-300 nm, 301-1500 nm, 10-150 μm), urethane (50-300 nm, 301-1500 nm), thiourethane, PET (5,10 wt), PS, PC, urea, melamine, acrylic melamine) shown in Tables 2 and 3, the number of best evaluations (acrylic, urethane, thiourethane, PS, PC, urea, melamine, acrylic melamine: ◯, PET: ◎) and the number of worst evaluations (acrylic, urethane, thiourethane, PET, PS, PC, urea, melamine, acrylic melamine: ×) were counted, and the overall compatibility (transparency) of each compound with the resin was evaluated according to the criteria in Table 12. The results are shown in Table 13.

[0428] As a result, compounds with a rating of 1 or higher were 13a Compounds with carbon numbers of 1 to 18 and melting points of 91°C or less (compounds 6, 7, 8, 9, 10, 11, 12, and 13), and compounds with a rating of 2 or higher are R 13a Compounds with carbon numbers of 1 to 12 and melting points of 91°C or less (compounds 6, 7, 8, 9, 10, 12, and 13), and compounds with a rating of 3 or higher are R 13a Compounds having 1 to 10 carbon atoms and a melting point of 91°C or less (compounds 6, 7, 8, 9, and 12) or R 13a The carbon number is 1 to 12, the melting point is 91°C or less, and R 2a , R 4a Compounds with methyl and t-butyl groups as substituents (compounds 6, 7, 8, 9, and 10), with a rating of 4 or higher, are R 13a The carbon number is 1 to 12, the melting point is 91°C or less, and R 2a , R 4a Compounds with methyl and t-butyl groups as substituents (compounds 6, 7, 8, 9, and 10), with a rating of 5 or higher, are R 13a The carbon number is 4 to 10, the melting point is 91°C or less, and R 2a , R 4a Compounds with methyl and t-butyl groups as substituents (compounds 6, 7, 8, and 9), with a rating of 6 or higher, are R 13a Compounds 7, 8, and 9, which have 6 to 10 carbon atoms and a melting point of less than 70°C, and compounds 2a and 4a with methyl and t-butyl substituents, respectively, are included in this category. The compatibility (transparency) with the matrix resin depends on both the number of carbon atoms in the alkyl group of formula (i-2) in the benzotriazole skeleton of formula (I) as the additive structure and the melting point of the compound, rather than on either one of them (compound 12 (carbon number: 8, melting point: 80 to 81°C), which has 10 or less carbon atoms but a melting point of 70°C or more: rated 3, and compound 13 (carbon number: 12, melting point: 64 to 66°C), which has a melting point of less than 70°C but has 10 or more carbon atoms: rated 2, are not generally rated as good).

[0429] Also, R 13a The number of carbon atoms in R is the same. 1a -R 5a Compound 8 (R 13a Number of carbon atoms: 8, 2a, 4a substituents: methyl group, t-butyl group) and 12 (R13a Number of carbon atoms: 8, R 2a , R 4a Substituents: t-butyl group, t-butyl group) and compound 10 (R 13a Number of carbon atoms: 12, R 2a , R 4a Substituents: methyl group, t-butyl group) and 13 (R 13a Number of carbon atoms: 12, R 2a , R 4a When comparing the substituents of R and R (t-butyl group, t-butyl group), compound 8 showed better compatibility (transparency) than compound 12 with the thermoplastic resin PET and the thermosetting resins urea, melamine, and acrylic melamine resins, while compound 10 showed better compatibility (transparency) than compound 13 with the thermoplastic resins thiourethane, PET, and the thermosetting resins melamine and acrylic melamine (Figure 17). The above evaluations were also high. In other words, the compatibility (transparency) of the resins was higher than that of compound 12. 2a , R 4a Compounds with methyl and t-butyl groups as substituents of R showed good overall tendency. 13a Compounds with 12 or less carbon atoms (compounds 6, 7, 8, 9, and 10), and further compounds with 4 to 10 carbon atoms (compounds 6, 7, 8, and 9), and especially compounds 7, 8, and 9 with 6 to 10 carbon atoms, showed good compatibility (transparency) with all resins, regardless of whether they were thermosetting or thermoplastic resins, such as acrylic, urethane, thiourethane, PET, PS, PC, urea, and melamine.

[0430] Furthermore, compounds 15 to 21 having thioether groups including branched aliphatic hydrocarbon groups, cyclic aliphatic hydrocarbon groups, alkene group-containing aliphatic hydrocarbon groups, aromatic groups, and oxygen-containing aliphatic hydrocarbon groups, etc., showed compatibility (transparency) with PS and PC, suggesting the effects of the introduction of sulfur-containing groups and the melting point, etc. (2) Film thickness The film thickness was obtained by measuring the cross section of the film using a tabletop microscope (Miniscope TM3000, Hitachi High-Tech Corporation) or by measuring the reflectance of the film using a reflectance meter (USPM-RU, Olympus Corporation) and performing fitting analysis of the obtained reflectance waveform using the Hartmann dispersion equation. (3) Refractive index The refractive index of the film was determined by measuring the one-side reflectance (λ=589 nm) (Tables 1, 2, 5, 6, and 7).

[0431] The acrylic resin films to which the compounds of the present invention were added (compounds 1, 3, 4, 5, 8, 10, 14, 22, 23, 24, 25, 26, 27, and 28: refractive index 1.5178 to 1.5914) had higher refractive indexes than the additive-free film (1.4985) of Comparative Example 1. Compounds 1, 3, 4, 8, 10, and 14, which have sulfur-containing groups, had higher refractive indexes than compound 5, which does not have a sulfur-containing group, suggesting the effect of the compounds of the present invention having a sulfur-containing group in increasing the refractive index.

[0432] From these results, it was confirmed that the compounds of the examples cut the wavelengths of the ultraviolet region around 250 to 400 nm and transmit the wavelengths of 450 to 500 nm (visible region), and that they have excellent ultraviolet absorption ability of 315 to 400 nm (UV-A region) that affects the photodegradation of organic substances, and cut ultraviolet rays up to the region around 400 nm. Therefore, the additive of the present invention is useful because it can prevent deterioration and discoloration of the resin that becomes the matrix. In addition, the effect of increasing the refractive index of the resin film was also confirmed. And even when added in an amount of 0.4 to 50 wt% based on the total of the resin and the additive, the film was transparent and did not discolor, and it was confirmed that the compounds of the examples have high solubility in the resin and can be used at high concentrations while maintaining transparency.

[0433] [Table 1]

[0434] [Table 2]

[0435] [Table 3]

[0436] [Table 4]

[0437] [Table 5]

[0438] [Table 6]

[0439] [Table 7]

[0440] [Table 8]

[0441] [Table 9]

[0442] [Table 10]

[0443] [Table 11]

[0444] [Table 12]

[0445] [Table 13]

[0446] 3. Evaluation of plastic lenses (Making plastic lenses) Resins were prepared by adding the additive of the present invention and a conventional ultraviolet absorbent. In the following examples and comparative examples, the amount of each ultraviolet absorbent added was adjusted so that the transmittance of a 2 mm thick flat lens at 420 nm was as close as possible for the same type of resin. <Example 71> 0.49g of compound 8, 0.1g of Stefan Zerec UN, 0.04g of dibutyltin dichloride, and 50.8g of a mixture of 2,5-bis(isocyanatomethyl)-bicyclo[2,2,1]heptane and 2,6-bis(isocyanatomethyl)-bicyclo[2,2,1]heptane were placed in a flask and stirred at 25°C for 1 hour to completely dissolve. Then, 22.4g of pentaerythritol tetrakis(3-mercaptopropionate) and 26.8g of 1,2-bis[(2-mercaptoethyl)thio]-3-mercaptopropane were added to the mixture and mixed at 25°C for 30 minutes. In addition, the compound 8 was contained in the prepared solution at 0.49% by weight relative to the total weight of the polymerizable compounds.

[0447] This mixed liquid was degassed at 0.3 mmHg or less for 1 hour, filtered with a 5 μm PTFE filter, and poured into a mold consisting of a flat glass mold with a center thickness of 2 mm and a diameter of 80 mm and a tape. The mold was gradually heated from 25°C to 130°C, held at 130°C for 2 hours, and then cooled to room temperature. It took 18 hours from the start of the temperature increase to the cooling. After the polymerization was completed, the obtained molded body was released from the mold, and the flat lens was annealed at 130°C for 2 hours. <Example 72> A flat lens having a thickness of 2 mm was obtained in the same manner as in Example 71, except that 0.53 g (0.53% by weight based on the total weight of the polymerizable compounds) of Compound 8 in Example 71 was added. <Example 73> 0.53 g of compound 8 (0.53% by weight based on the total weight of the polymerizable compounds), 0.1 g of Stefan Zerec UN, 0.2 g of dibutyltin dichloride, and 58.9 g of dicyclohexylmethane-4,4'-diisocyanate were placed in a flask and completely dissolved by stirring at 25°C for 1 hour. After that, 41.1 g of a mixture mainly composed of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane was added to the mixture and mixed at 25°C for 30 minutes.

[0448] A 2 mm thick flat lens was obtained in the same manner as in Example 71, except for the preparation of the mixed solution. <Example 74> 0.27 g of compound 8 (0.27% by weight based on the total weight of the polymerizable compounds), 0.1 g of Stefan Zelec UN, 0.006 g of dibutyltin dichloride, and 50.6 g of m-xylylene diisocyanate were placed in a flask and completely dissolved by stirring at 25° C. for 1 hour. After that, 49.4 g of a mixture mainly composed of 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane was added to the mixture and mixed at 25° C. for 30 minutes.

[0449] A 2 mm thick flat lens was obtained in the same manner as in Example 71, except for the preparation of the mixed solution. <Example 75> Into a flask, 0.23 g of compound 8 (0.23% by weight relative to the total weight of the polymerizable compounds), 71 g of bis(β-epithiopropyl)sulfide, 23 g of sulfur, and 2.2 g of (2-mercaptoethyl)sulfide were placed, and the mixture was stirred at 60° C. for 30 minutes. Then, 0.14 g of 2-mercapto-1-methylimidazole was placed, and the mixture was degassed at 0.3 mmHg or less for 10 minutes, and then further stirred at 60° C. for 120 minutes, and then cooled to 30° C. over 40 minutes. To the resulting solution, a solution obtained by dissolving 0.012 g of triethylbenzylammonium chloride and 0.01 g of dibutyltin dichloride in 3.8 g of (2-mercaptoethyl)sulfide was dropped, and the mixture was degassed at 0.3 mmHg or less for 20 minutes. The solution was filtered through a 5 μm PTFE filter and poured into a mold consisting of a flat glass mold with a center thickness of 2 mm and a diameter of 80 mm and a tape. The mold was gradually heated from 25°C to 110°C, held at 110°C for 2 hours, and then cooled to room temperature. It took 18 hours from the start of the temperature increase to the cooling. After the polymerization was completed, the obtained molded body was released from the mold, and the flat lens was annealed at 110°C for 2 hours. <Example 76> A flat lens having a thickness of 2 mm was obtained in the same manner as in Example 71, except that compound 8 in Example 71 was changed to compound 10 and 0.56 g (0.56% by weight based on the total weight of the polymerizable compounds) was added. <Example 77> A 2 mm thick flat lens was obtained in the same manner as in Example 71, except that compound 8 in Example 71 was changed to compound 14 and 0.58 g (0.58 wt % based on the total weight of the polymerizable compounds) was added. <Comparative Example 14> A 2 mm thick flat lens was obtained in the same manner as in Example 71, except that compound 8 in Example 71 was changed to 2-(2-hydroxy-3-t-butyl-5-methylphenyl)-chlorobenzotriazole (compound 36) and 0.75 g (0.75 wt % based on the total weight of the polymerizable compounds) was added. <Comparative Example 15> A flat lens having a thickness of 2 mm was obtained in the same manner as in Example 71, except that 0.85 g (0.85% by weight based on the total weight of the polymerizable compounds) of Compound 36 of Comparative Example 14 was added. <Comparative Example 16> A 2 mm thick flat lens was obtained in the same manner as in Example 71, except that compound 8 in Example 73 was changed to 2-(2-hydroxy-3-t-butyl-5-methylphenyl)-chlorobenzotriazole (compound 36) and 0.75 g (0.75 wt % based on the total weight of the polymerizable compounds) was added. <Comparative Example 17> A 2 mm thick flat lens was obtained in the same manner as in Example 71, except that compound 8 in Example 74 was changed to 2-(2-hydroxy-3-t-butyl-5-methylphenyl)-chlorobenzotriazole (compound 36) and 0.50 g (0.50 wt % relative to the total weight of the polymerizable compounds) was added. <Comparative Example 18> A 2 mm thick flat lens was obtained in the same manner as in Example 75, except that compound 8 in Example 75 was changed to 2-(2-hydroxy-3-t-butyl-5-methylphenyl)-chlorobenzotriazole (compound 36), and 0.30 g (0.30 wt % based on the total weight of the polymerizable compounds) was added. (1) Transmittance, yellowness index (YI value), visual transmittance The sample lenses produced in the examples and comparative examples were measured for spectral transmittance from 350 to 800 nm, yellowness index (YI value), and luminous transmittance using a UV-visible spectrophotometer (U-4100 manufactured by Hitachi High-Technologies Corporation). The yellowness index and luminous transmittance were measured using a D65 light source and a 2-degree visual field. (2) Appearance evaluation of sample lenses The sample lenses produced were visually compared and confirmed for yellowness between the sample lenses of the examples and comparative examples, which are made of the same resin material and have similar transmittance at around 420 nm. This is because the yellowness inherent in the resin itself differs depending on the type of resin, so it is not possible to accurately compare the yellowness caused by adding an ultraviolet absorber to another resin. The lenses compared are, in detail, Example 71 and Comparative Example 14, Example 72 and Comparative Example 15, Example 73 and Comparative Example 16, Example 74 and Comparative Example 17, Example 75 and Comparative Example 18, Example 76 and Comparative Example 14, and Example 77 and Comparative Example 14. The appearance was evaluated according to the following criteria. In addition, the precipitation of the ultraviolet absorber from the resin and the transparency were visually confirmed. Yellowness: ○: Nearly colorless, ×: Yellow The YI value and the results of the appearance evaluation are shown in Table 14, and the measurement results of the transmission spectrum are shown in Figs.

[0450] When an ultraviolet absorbing agent is used to cut off the wavelength region of 400 to 420 nm, depending on the type of ultraviolet absorbing agent, the resin may turn yellow, or may not completely dissolve in the resin of the plastic lens and precipitate, causing the resin to become cloudy. For example, Japanese Patent No. 4334633 describes that when an ultraviolet absorbing agent with a molecular weight of more than 360 is used, its solubility in the raw monomer decreases, and even when the amount of the ultraviolet absorbing agent is 5 parts by weight or less, it precipitates on the surface of the plastic lens, and the limit amount at which it does not precipitate does not have sufficient ultraviolet absorbing ability, making it difficult to obtain a plastic lens that can sufficiently absorb ultraviolet rays with a wavelength of 380 to 400 nm. However, due to the structural characteristics of the additive of the present invention, compounds 8, 10, and 14, although their molecular weights exceed 360 compared to the molecular weight of compound 36 of 316, are well dissolved in the monomer like compound 36, and do not precipitate on the surface of the obtained plastic lens, and it has been confirmed that the structure of the ultraviolet absorbing agent of the present application expresses affinity to monomers and plastic lenses.

[0451] Furthermore, compared with lenses using 2-(2-hydroxy-3-t-butyl-5-methylphenyl)-chlorobenzotriazole, plastic lenses using the ultraviolet absorber represented by formula (I) more efficiently absorb light with wavelengths of 400 to 420 nm with a smaller amount of additive, have good transmittance for light with wavelengths of around 420 nm or longer while suppressing adverse effects on the eyes, and suppress yellowing of the plastic lenses, resulting in lenses with excellent appearance.

[0452] Therefore, it was confirmed that the additive of the present invention has good compatibility with the matrix resin and can fully exhibit performance such as ultraviolet absorption and high refractive index while maintaining high transparency.

[0453] [Table 14]

[0454] 4. Evaluation of fixation of additives with reactive functional groups to resin 0.022 g of isocyanate (HC-210, manufactured by Nippon Polyurethane Co., Ltd.), 0.078 g of polyol (ON-H37, manufactured by Nippon Polyurethane Co., Ltd.), and 0.002 g of compounds 1 and 20 were each homogeneously mixed with 12 g of chloroform, and approximately 1 mL of each was spin-coated onto a glass substrate at 1500 rpm for 20 seconds. The chloroform was then removed in a 45°C oven, and the substrate was then heated at 100°C for 3 hours to produce a urethane film.

[0455] The obtained film was immersed in warm water at 70° C., and the absorbance at the maximum absorption wavelength of Compounds 1 and 20 was measured at regular intervals.

[0456] The absorbance retention (%) was calculated as [(absorbance after 10 and 40 hours / initial absorbance)×100]. When the absorbance retention was measured after 10 hours and 40 hours for the compounds of Examples 1 and 20, the transparency was maintained and the absorbance retention of the film was almost the initial value.

[0457] 2.5g of methyl methacrylate, 0.05g of compound 17, 10g of toluene as a solvent, 10g of methyl ethyl ketone (MEK), and 0.025g of 1,1'-azobis(cyclohexane-1-carbonitrile) as a polymerization initiator were charged, and after stirring for 1 hour under a nitrogen atmosphere, the polymerization reaction was carried out at a reaction temperature of 88 to 91 ° C. for 10 hours under heating and refluxing. 250g of MEK was added to the obtained copolymer solution, and the solution was dropped into 2500g of methanol using a dropping funnel over 1 hour to precipitate copolymer crystals. Next, filtration, purification, and drying under reduced pressure were performed to obtain 2.12g of methacrylic resin.

[0458] 0.10 g of the obtained methacrylic resin was heated and melted at 280° C., then dropped onto a slide glass substrate, quickly spread, and air-cooled to form a film.

[0459] The obtained film was immersed in warm water at 70°C, and the absorbance at the maximum absorption wavelength of Compound 17 was measured every 10 and 40 hours. The absorbance retention was measured in the same manner as above. It was found that the transparency was maintained and the absorbance retention of the film was almost the same as the initial value.

[0460] In other words, it was confirmed that there was no elution of the additives having reactive functional groups to the monomer or resin, the additives reacted with the monomer and were fixed in the resin, and did not bleed out, maintaining transparency and allowing each of the functions such as ultraviolet absorption ability and high refractive index to be maintained for a long period of time.

Claims

1. The following formula (III): 【Chemistry 1】 (In the formula, R 1c ~R 10c each independently represents the following formula (iii-1): 【Chemistry 2】 (In formula (iii-1), R 11c represents an alkylene group having 10 or less carbon atoms, and t represents an integer of 0 or 1.) represents a monovalent group selected from a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom. R 1c ~R 10c At least one of the groups represented by the formula (iii-1) is a monovalent sulfur-containing group represented by the formula (iii-2).

2. The following formula (III): 【Chemistry 3】 (In the formula, R 1c ~R 10c each independently represents the following formula (iii-2): 【Chemistry 4】 (In formula (iii-2), R 13c When v is 2 or more, each independently represents a divalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted or a carbon-carbon bond may be interrupted by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom; R 14c represents a monovalent hydrocarbon group having 1 to 20 carbon atoms in which a hydrogen atom may be substituted or a carbon-carbon bond may be interrupted by a monovalent or divalent group selected from an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a halogen atom, provided that the sulfur atom S in formula (iii-2) is a thioether group. 13c and R 14c The total number of carbon atoms in is 25 or less. v is an integer of 0 to 3. R is a monovalent sulfur-containing group represented by the formula (I), a hydrogen atom, a hydrocarbon group having 1 to 10 carbon atoms, an aromatic group, an unsaturated group, a sulfur-containing group, an oxygen-containing group, a phosphorus-containing group, an alicyclic group, and a monovalent group selected from a halogen atom. 1c ~R 10c At least one of the groups represented by the formula (iii-1) is a monovalent sulfur-containing group represented by the formula (iii-2).

3. The additive described in claim 2, wherein the monovalent sulfur-containing group represented by formula (iii-2) has v R 13c which is an alkylene group having 18 or less carbon atoms and v R 14c which is an alkyl group having 18 or less carbon atoms.

4. The additive according to any one of claims 1 to 3, wherein the matrix is ​​a transparent resin.

5. A resin part containing the additive described in any one of claims 1 to 3 in a matrix resin.

6. A transparent resin part containing an additive according to any one of claims 1 to 3 in a matrix resin.

Citation Information

Patent Citations

  • Twooway function stabilizer compound

    JP1979132546A

  • 5-Thio-substituted benzotriazole UV absorber and stabilized composition

    JP1994505744A

  • Thioether-substituted hydroxybenzophenone and stabilized composition

    JP1995285927A

  • UV absorber

    JP2005504047A

  • Compound, polymerizable compound, polymer material, and film

    JP2012184168A