Photocatalyst and method for producing the same

A photocatalyst with a specific semiconductor and gold support efficiently produces ethane from methane at low temperatures using sunlight, addressing energy inefficiencies and safety concerns of traditional methods while achieving high ethane production rates.

JP7578269B2Active Publication Date: 2024-11-06NAT INST FOR MATERIALS SCI
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020187671
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-11
Publication Date
2024-11-06
Estimated Expiration
2040-11-11

AI Technical Summary

Technical Problem

Existing methods for producing ethane from methane require high temperatures, which are energy-inefficient and pose safety risks, and existing photocatalytic methods have low efficiency and are limited by the wavelength of usable light.

Method used

A photocatalyst composed of a semiconductor with a band gap of 2.8 to 4.4 eV and supported gold particles, preferably a nanocomposite of zinc oxide and titanium oxide, is used to produce ethane from methane under sunlight wavelengths, with specific ratios and conditions for optimal performance.

Benefits of technology

The method achieves high ethane production efficiency using safe, inexpensive, and easily handled sunlight wavelengths, with ethane production rates exceeding 85% and amounts up to 5000 μmol g-1 h-1.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578269000007
    Figure 0007578269000007
  • Figure 0007578269000008
    Figure 0007578269000008
  • Figure 0007578269000009
    Figure 0007578269000009
Patent Text Reader

Abstract

To provide a manufacturing method for obtaining ethane from methane gas with high safety and high production volume and production ratio, and a photocatalyst that becomes a key to the manufacturing method.SOLUTION: A photocatalyst includes a semiconductor whose band gap is 2.8-4.4 eV, and gold(Au) fine particles carried on the semiconductor. The semiconductor is composed of one or more selected from the group consisting of zinc oxide and titanic oxide. Ethane is manufacturable by bringing the photocatalyst into contact with gas containing methane and oxygen under irradiation with light having a wavelength of 280 nm or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photocatalyst, a method for producing the photocatalyst, and a method for producing ethane using the photocatalyst and methane. [Background technology]

[0002] Ethane is the main raw material for synthesizing ethylene, which is the main raw material for industrially useful materials such as polyethylene and vinyl chloride, and is an industrially important saturated hydrocarbon (alkane) with added value. Ethane is contained in natural gas and crude oil, and can also be obtained by fractional distillation of these fossil fuels. However, the proportion of ethane contained in crude oil and natural gas is small, so the efficiency is insufficient. Therefore, the industrial synthesis of ethane (C2H6) by a methane coupling reaction using methane (CH4), the main component of natural gas, is being researched.

[0003] Methane is highly symmetric and has a very high bond dissociation energy of 439 kJ / mol between CH+, so high temperatures are required to dissociate the hydrogen atoms. Therefore, the direct production of ethane from methane via the dissociation also requires high temperatures. For example, it has been reported that ethane and ethylene can be produced by using Li2SrGeO4 as a catalyst and heating methane to 800°C (see Patent Document 1). It has also been reported that a catalyst in which manganese oxide and alkaline tungsten oxide are supported on silicon oxide (Na2WO4-Mn / SiO2) can also convert methane to ethane at high temperatures of 780°C or higher (see Non-Patent Document 1).

[0004] Direct conversion of methane to ethane using a thermal catalyst like this requires high-temperature heating of around 800°C, but from the standpoint of energy efficiency and ensuring the safety of the production plant, it is preferable to carry out the reaction at lower temperatures. Methods using photocatalysis have been proposed as a method for converting methane to ethane at lower temperatures. For example, it has been reported that ethane can be produced from methane and water vapor at 25°C under irradiation of 254 nm ultraviolet light using a photocatalyst made of platinum (Pt) supported on gallium oxide (Ga2O3) (see Non-Patent Document 2). Gallium oxide has a band gap of 4.5 eV, and can only exhibit photocatalytic properties with light of 280 nm or less. However, most sunlight with wavelengths of 280 nm or less does not reach the earth's surface, and highly reactive ozone is also generated, so this photocatalytic material cannot effectively promote the ethane production reaction in the convenient wavelength range of sunlight. Another disadvantage is that the window material used during light irradiation is limited to expensive quartz and other materials.

[0005] It has been reported that platinum (Pt)-supported gallium (Ga)-doped titanium oxide photocatalyst can produce ethane from pure methane gas under irradiation with a xenon lamp. Since the photocatalytic conversion to ethane is possible under irradiation with a xenon lamp, it is believed that this photocatalyst can utilize sunlight to promote the ethane production reaction. However, this method has the problem that the methane conversion rate after 4 hours of light irradiation is 10% or less, and the activity is not high (see Non-Patent Document 3).

[0006] As described above, there are still many challenges to overcome in providing catalysts and methods for ethane production that function at relatively low temperatures (below 200°C) and in the wavelength range of sunlight, and have high methane conversion ethane production properties. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2020-54954 A [Patent Document 2] JP 2020-28821 A [Non-patent literature]

[0008] [Non-Patent Document 1] J.Mol.Catal.A, vol.245, pp272-277(2006). [Non-Patent Document 2] Chem.Commun.,vol.56,pp6348-6351(2020). [Non-Patent Document 3] J.American Chemical Society,vol.141,pp6592-6600(2019). Summary of the Invention [Problem to be solved by the invention]

[0009] As mentioned in the background, ethane is an important industrial raw material, but the amount contained in underground resources such as natural gas is limited. For this reason, ethane production using the coupling reaction of methane, which is abundant in natural gas, has been considered. However, as described above, methane is highly symmetric and stable, and therefore a high temperature of about 800°C is required to carry out the methane coupling reaction using a thermal catalyst, as shown in Patent Document 1. From the standpoints of energy efficiency, durability of the reaction vessel, and safety of handling high temperatures with respect to flammable materials, there has been a demand for a method for producing ethane at a lower temperature.

[0010] One method for producing ethane at low temperatures is to use a photocatalyst, but as mentioned in the background section, this method has issues with respect to the availability of inexpensive and easy-to-handle wavelength bands and the efficiency of ethane production.

[0011] The present invention aims to provide a production method for efficiently producing ethane from methane gas by using light in the solar wavelength range, which is safe, inexpensive, and easy to handle, a photocatalyst that is a key component of the production method, and a method for producing the photocatalyst. [Means for solving the problem]

[0012] The configuration of the present invention for solving the problems is shown below. (Configuration 1) A semiconductor having a band gap of 2.8 eV or more and 4.4 eV or less, and gold particles (Au particles) supported on the semiconductor, The semiconductor is at least one selected from the group consisting of zinc oxide and titanium oxide, and is a photocatalyst for producing ethane from methane. (Configuration 2) The photocatalyst according to embodiment 1, wherein the semiconductor is a nanocomposite of ZnO and TiO2. (Configuration 3) 3. The photocatalyst according to claim 2, wherein a molar ratio of the ZnO to the TiO2 is 0.5 or more and 8 or less. (Configuration 4) 3. The photocatalyst according to claim 2, wherein a molar ratio of the ZnO to the TiO2 is 0.5 or more and 4 or less. (Configuration 5) 5. The photocatalyst according to any one of configurations 1 to 4, wherein a ratio of the Au fine particles to the photocatalyst is 0.1% by weight or more and 2.0% by weight or less. (Configuration 6) 5. The photocatalyst according to any one of configurations 1 to 4, wherein a ratio of the Au fine particles to the photocatalyst is 1.0% by weight or more and 2.0% by weight or less. (Configuration 7) 7. The photocatalyst according to any one of configurations 1 to 6, wherein the Au fine particles have a particle diameter of 2 nm or more and 5 nm or less. (Configuration 8) 7. The photocatalyst according to any one of configurations 1 to 6, wherein the Au fine particles have a particle diameter of 2.3 nm or more and 3.8 nm or less. (Configuration 9) Providing a layered hydroxide containing ZnTi ions; heat-treating the layered hydroxide in the presence of oxygen to produce a composite of ZnO and TiO2; suspending the composite in an aqueous solution to prepare an aqueous suspension containing ZnO and TiO; adding an HAuCl4 aqueous solution to the aqueous suspension to prepare an HAuCl4-added aqueous solution; A method for producing a photocatalyst, comprising adding a reducing agent to the HAuCl4-added aqueous solution, and then drying the solution to produce a photocatalyst. (Configuration 10) 10. The method for producing a photocatalyst according to claim 9, wherein the temperature of the heat treatment is 200° C. or higher and 800° C. or lower. (Configuration 11) 11. The method for producing a photocatalyst according to claim 9 or 10, wherein the reducing agent is an aqueous NaBH4 solution. (Configuration 12) A method for producing ethane, comprising contacting a gas containing methane and oxygen with the photocatalyst according to any one of configurations 1 to 8 under irradiation with light having a wavelength of 280 nm or more to produce ethane. (Configuration 13) 13. The method for producing ethane according to claim 12, wherein the gas is contacted with the photocatalyst as a gas stream. (Configuration 14) 13. The method for producing ethane according to claim 12, wherein the gas is sealed in a reaction chamber and contacted with the photocatalyst. (Configuration 15) 15. The method for producing ethane according to any one of claims 12 to 14, wherein a molar ratio of the methane to the oxygen is 2 or more and 1000 or less. (Configuration 16) 15. The method for producing ethane according to any one of claims 12 to 14, wherein a molar ratio of the methane to the oxygen is 10 or more and 1,000 or less. (Configuration 17) 17. The method for producing ethane according to any one of claims 12 to 16, wherein the oxygen-containing gas is air. (Configuration 18) 18. The method for producing ethane according to any one of configurations 12 to 17, wherein the light is light having a wavelength range of 280 nm or more and 500 nm or less. Effect of the Invention

[0013] According to the present invention, there are provided a production method for obtaining highly efficient production of ethane from methane gas by using a safe, inexpensive and easy-to-handle solar wavelength band, a photocatalyst that is a key component of the production method, and a method for producing the photocatalyst. [Brief description of the drawings]

[0014] [Figure 1] 1 is XRD measurement data showing the material structure of the present invention. [Diagram 2]FIG. 2 is a characteristic diagram showing the particle size distribution of supported metal Au in the material of the present invention. [Diagram 3] 1 is a TEM photograph of a material of the present invention. [Figure 4] 1 is a high-resolution TEM (HRTEM) photograph showing the material structure of the present invention. [Diagram 5] 1 is a STEM photograph of a material of the present invention. [Figure 6] This is an example of EDX measurement data of the material of the present invention, in which Zn, O, Ti and Au were detected. [Figure 7] FIG. 1 is a flow chart showing the manufacturing process of the material of the present invention. [Figure 8] FIG. 2 is an explanatory diagram showing an outline of the device in a cross-sectional view. [Figure 9] FIG. 2 is a characteristic diagram showing the dependency of ethane production amount on supported metal. [Figure 10] FIG. 1 is a characteristic diagram showing the dependency of ethane production ratio on supported metal. [Figure 11] FIG. 1 is a characteristic diagram showing the dependency of ethane production amount on the amount of Au supported. [Figure 12] FIG. 1 is a characteristic diagram showing the effect of the nanocomposite on ethane production. [Figure 13] FIG. 1 is a characteristic diagram showing the dependency of ethane production amount on material composition. [Figure 14] FIG. 2 is a characteristic diagram showing the dependency of the ethane production amount and production ratio on the methane ratio relative to oxygen. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the present invention will be described with reference to the drawings.

[0016] (First embodiment) <Photocatalyst> The photocatalyst of the present invention is composed of a semiconductor as a main catalyst and fine particles of gold (Au) as a promoter. The semiconductor that constitutes the main catalyst is one or more selected from the group consisting of zinc oxide and titanium oxide, each having a band gap of 2.8 eV to 4.4 eV. The band gaps of anatase-type titanium dioxide (TiO2), rutile-type TiO2, brookite-type TiO2, and zinc oxide (ZnO) have been reported to be 3.2 eV, 3.0 eV, 3.2 eV, and 3.3 eV, respectively. Here, as for TiO2, anatase-type and brookite-type are more active catalytically than rutile-type, so anatase-type and brookite-type are preferably used. The semiconductor may be doped with one or more metals selected from the group consisting of tantalum (Ta), niobium (Nb), zirconium (Zr), vanadium (V), chromium (Cr), iron (Fe), gallium (Ga) and indium (In). This doping accelerates the reaction.

[0017] 2.8 eV is equivalent to a light wavelength of approximately 443 nm, and 4.4 eV is approximately 282 nm, so in the sunlight wavelength band, this semiconductor generates electrons and holes with strong oxidizing power. Most sunlight that reaches the Earth's surface has a wavelength of 280 nm or more. In the sunlight wavelength band considered here (280 nm or more and 500 nm or less), light attenuation by air is low, and inexpensive glass can be used as the window material for light irradiation, which is necessary when producing ethane at plants. In addition, it will be possible to use highly efficient and inexpensive Xe lamps or LEDs for the light irradiated to the photocatalyst.

[0018] In order to increase the efficiency of ethane production, the main catalyst is preferably made of multiple semiconductors, for example, ZnO and TiO2, and more preferably a nanocomposite of ZnO and TiO2. Here, the term "nanocomposite" refers to a composite material in which a first component material is finely divided into particles having a size of 1 nm to 100 nm and is attached in a highly dispersed manner to a second component material.

[0019] When ZnO and TiO2 are used as the main catalyst, in order to obtain a high amount of ethane production (to obtain a high efficiency of ethane production), the molar ratio of ZnO to TiO2 is preferably 0.5 to 8, and more preferably 0.5 to 4.

[0020] The Au microparticles, which act as a co-catalyst, are supported on the semiconductor, which acts as the main catalyst. The Au must be in the form of microparticles so that sufficient light can reach the semiconductor.

[0021] In order to obtain a high ethane production amount (high ethane production efficiency), the particle size of Au is preferably 2 nm to 5 nm, more preferably 2.3 nm to 3.8 nm. Here, the particle size of Au is defined as the diameter of an Au particle when it is approximated by a sphere of equal volume. Methods for measuring the particle size include dynamic light scattering (photon correlation method), static light scattering (laser diffraction / scattering method), calculation from SEM (Scanning Electron Microscope) images, and calculation from TEM (Transmission Electron Microscope) images.

[0022] The ratio of Au particles to the photocatalyst (main catalyst and co-catalyst) is preferably 0.1% by weight or more and 2.0% by weight or less in terms of the ethane production ratio. When the ratio of Au particles is in this range, a high ethane production rate of 85% or more can be obtained. In addition, when the ratio of Au particles is in this range, the amount of ethane produced is about 2.5 mmol g -1 h -1 This is a higher value than the above. The loading ratio of Au fine particles is more preferably 1.0% by weight or more and 2.0% by weight or less. When the loading ratio is 1.0% by weight or more and 2.0% by weight or less, the loading ratio is 4.8 mmol g -1 h -1 Ethane production of more than 1000 times higher can be achieved. Since the Au particles are mainly supported on the surface of the main catalyst, if the ratio of the Au particles supported is too high, the light blocking effect of the Au particles makes it difficult for light to reach the main catalyst, and the amount of ethane produced decreases.

[0023] The photocatalyst (main catalyst and co-catalyst) of the present invention may be supported on a carrier. The form in which the photocatalyst is supported on the carrier is not particularly limited, but it is preferable that the photocatalyst is supported in a highly dispersed state.

[0024] The carrier is not particularly limited, and a known carrier can be used. The carrier preferably has a large specific surface area, and more specifically, zeolite, silica, metal-organic framework (MOF), activated carbon, etc. can be mentioned.

[0025] The content of the carrier in the photocatalytic material is not particularly limited and may be appropriately selected depending on the application, but it is preferably from 5% by weight to 95% by weight, more preferably from 5% by weight to 40% by weight, and even more preferably from 10% by weight to 30% by weight, based on the total mass of the photocatalytic material (photocatalyst and carrier).

[0026] The ethane production mechanism is as follows: When the above-mentioned semiconductor photocatalysts, such as titanium oxide or zinc oxide, are irradiated with sunlight wavelengths, electrons and holes with strong oxidizing power are generated, and the holes dissociate the hydrogen atoms in the methane molecules to generate methyl radicals (CH3 radicals). These two radicals couple to generate ethane. The generated electrons then move onto the supported co-catalyst (Au fine particles), promoting charge separation and further promoting the generation of methyl radicals. In particular, the above-mentioned supported co-catalysts have a weaker adsorption power for methyl radicals, which promotes the coupling reaction.

[0027] <Photocatalyst manufacturing method> The method for producing the photocatalyst according to the present invention is not particularly limited to a specific method, and various known methods can be applied. For example, a method in which a precursor compound such as a metal alkoxide or a metal salt (which may contain a precursor compound of a promoter) is heated to hydrolyze, washed, and synthesized can be mentioned. The photocatalyst thus obtained may be crushed by a method such as a ball mill and, if necessary, reduced to fine particles before use. Examples of the method for supporting the promoter on the main catalyst include a photoprecipitation method and an impregnation method.

[0028] The following method can be used to manufacture a photocatalyst in which a nanocomposite of ZnO and TiO2 is used as the main catalyst and Au is used as the co-catalyst. This method will be described with reference to the flow chart of FIG. First, layered hydroxides containing ZnTi ions (ZnTi-LDHs) are prepared (Step S11 in FIG. 7). Next, the layered hydroxide is heat-treated in the presence of oxygen to produce a composite of ZnO and TiO2 (step S12). Here, oxygen may be supplied in the form of air. The heat treatment temperature is preferably 200°C or higher and 800°C or lower. Under these conditions, the composite can be produced in a high yield. Thereafter, the composite is suspended in an aqueous solution to prepare an aqueous suspension containing ZnO and TiO2 (step S13). Next, a HAuCl4 aqueous solution is added to the suspension to prepare a HAuCl4-added aqueous solution (step S14). The amount of HAuCl4 in the HAuCl4 aqueous solution can be 0.1 g to 100 g per 1 L of aqueous solution, and the amount of the HAuCl4 aqueous solution added to the suspension can be 0.01 wt % to 10 wt % based on the weight of the ZnO-TiO2 photocatalyst. Under these conditions, a photocatalyst using a nanocomposite as a main catalyst can be prepared with a high yield. After that, a reducing agent is added to the HAuCl4-added aqueous solution, and finally, drying is performed (step S15). Through the above steps, a photocatalyst is produced in which a nanocomposite made of ZnO and TiO2 is used as the main catalyst and Au fine particles are supported as a co-catalyst. Here, examples of reducing agents include a NaBH4 aqueous solution, a formaldehyde solution, and a citric acid aqueous solution. Among these, a NaBH4 aqueous solution is preferably used due to its stability and ease of handling.

[0029] The photocatalyst made of a nanocomposite of ZnO and TiO2 carrying Au fine particles thus produced enables the production of ethane from methane in a high yield. In addition to the above, other methods for carrying Au fine particles include the photoprecipitation method.

[0030] <Production method of ethane> Ethane is produced by irradiating the photocatalyst of the present invention with light having a wavelength of 280 nm or more in the presence of a gas containing methane and oxygen. Here, the state of the gas containing methane and oxygen near the photocatalyst may be a gas flow or a gas in a stagnant state (static state), but a gas flow state makes it easier to control the residence time and reaction time, and makes it easier to increase the ethane production selectivity. On the other hand, a gas stagnant state (reaction in a static system) has the characteristic that the amount of methane used is easily reduced. It is possible to heat the catalyst at a temperature of 40°C or higher and 1000°C or lower as long as the catalytic activity is not reduced, but a high temperature of, for example, 1000°C is disadvantageous in terms of safety against explosions and the energy and equipment costs required for high-temperature heat treatment. Therefore, the temperature for heating is preferably 40°C or higher and 800°C or lower.

[0031] An overview of ethane production apparatus 101 is shown in Figure 8. Ethane production apparatus 101 includes photocatalyst 12 of the present invention installed in housing 11, window 13 that transmits irradiated light 14, gas inlet 15 and valve 17 for introducing methane gas 16 into housing 11, gas inlet 18 and valve 20 for introducing oxygen-containing gas 19 such as air into housing 11, and outlet 21 and valve 23 for ethane gas 22.

[0032] To make the gas containing methane and oxygen flow near the photocatalyst 12, the valves 17 and 20 are opened to continuously introduce the methane gas 16 from the gas inlet 15 and the gas containing oxygen 19 from the gas inlet 18, and the valve 23 is opened to take out the gas containing ethane 22 from the outlet 21. On the other hand, to make the gas containing methane and oxygen flow near the photocatalyst 12, the valves 17 and 20 are opened after the valve 23 is opened to introduce the methane gas 16 from the gas inlet 15 and the gas containing oxygen 19 from the gas inlet 18, and the methane gas 16 and the gas containing oxygen 19 are filled in the housing 11. When the gas is sufficiently filled, the valves 17, 20 and 23 are closed to make the housing 11 into a sealed space.

[0033] The irradiated light 14 is light in a wavelength range of 280 nm or more. Light with a wavelength shorter than 280 nm is not preferred because it has a small photocatalytic activity effect on the photocatalyst 12 of the present invention and is prone to generate ozone that induces the decomposition of ethane and inhibits the production of ethane. There are no particular limitations on the long wavelength side, but light with a wavelength exceeding 500 nm has a small photocatalytic activity effect on the photocatalyst 12 of the present invention. For this reason, the irradiated light 14 is preferably light in a wavelength range of 280 nm or more and 500 nm or less from the viewpoint of irradiation efficiency. In addition, since light in the wavelength range of 280 nm or more is used, window 13 can be made of inexpensive, easy-to-handle window materials such as soda glass, flint glass, crown glass, potassium lime glass, potassium lead glass, and borosilicate glass.

[0034] Examples of the oxygen-containing gas 19 include oxygen gas (O2 gas), air, a mixed gas of oxygen and argon, and a mixed gas of oxygen and nitrogen. Among these, air is preferably used because it is cheap, safe, and easy to handle.

[0035] The feed gas ratio, i.e., the ratio of oxygen to methane gas, has a significant effect on activity. If there is too much oxygen, methane is oxidized, which makes it easier for carbon dioxide to be produced, and ethane production is suppressed. On the other hand, if there is no oxygen, the methane coupling reaction does not occur easily, and in this case, ethane production is also suppressed. As a result of detailed investigations, the inventors have found that when the molar ratio of methane to oxygen is between 2 and 1000, the amount of ethane produced is large and the ratio of ethane produced is also high. In addition, when the molar ratio of methane to oxygen is between 10 and 1000, the production rate of ethane is about 5000 μmol g -1 h -1It was found that a particularly high amount of ethane was produced. Here, when the molar ratio of methane to oxygen is 10 or more and 1000 or less, the amount of ethane produced does not depend much on the molar ratio, but as the molar ratio increases within this range, the ethane production ratio increases monotonically. Therefore, the molar ratio of methane to oxygen is preferably 2 or more and 1000 or less, and more preferably 10 or more and 1000 or less. Furthermore, as a result of the investigation, it was found that nitrogen in the air does not have much effect on the amount of ethane produced or the ethane production ratio, so when air is used as the oxygen-containing gas, the molar ratio of methane to air is preferably 10 or more and 5000 or less, and more preferably 50 or more and 5000 or less.

[0036] <Photocatalyst Applications> When the photocatalyst of the present invention is irradiated with light in a wavelength range such as sunlight, it can selectively produce ethane through a methane coupling reaction. In other words, it is possible to produce ethane with high industrial added value from methane as a raw material without requiring high temperatures. It is also possible to combine the photocatalyst of the present invention with other materials and produce ethane using a Z-scheme reaction. In addition, by utilizing the above-mentioned photocatalytic reaction, for example, propane (C3H8) can be selectively produced from ethane (C2H6) as the starting material. n H (2n+2) ) is a saturated hydrocarbon with a higher carbon number (C m H (2m+2) ,m>n) can also be manufactured. EXAMPLES

[0037] The present invention will be described below based on examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed and used without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the examples shown below.

[0038] Example 1 In Example 1, photocatalyst 1 (1 wt % Au-supported ZnO / TiO2 (molar ratio of ZnO to TiO2: 4:1)) was prepared, and its material evaluation and ethane production characteristics were evaluated.

[0039] <Preparation of photocatalyst 1> Photocatalyst 1 (1 wt. % Au-loaded ZnO / TiO2 (molar ratio of ZnO to TiO2: 4:1) was prepared by the following method. Note that ZnO / TiO2 (molar ratio of ZnO to TiO2: a:b) may be referred to as ZnO / TiO2 (a / b) below as necessary. First, layered hydroxides containing ZnTi ions (ZnTi-LDHs) were prepared (Step S11 in FIG. 7). Specifically, 3 g of urea and 1.427 g of Zn(NO3) 6H2O were dissolved in 100 mL of deionized water, to which 131.59 μL of TiCl4 was added, and the mixture was heated at 100 °C for 48 hours. The solution was centrifuged, washed multiple times with deionized water, and then dried at 70 °C for 12 hours to obtain ZnTi-LDHs. Next, the mixture was calcined in air at 300° C. for 2 hours to obtain a ZnO / TiO 2 composite (step S12). 100 mg of the ZnO / TiO2 composite was suspended in 100 mL of deionized water under ultrasonic application to prepare a ZnO / TiO2 suspension (step S13), and then an HAuCl4 aqueous solution was added to the ZnO / TiO2 suspension and stirred at room temperature for 30 minutes to thoroughly mix the two (step S14). Then, an aqueous solution of the reducing agent NaBH4 was added thereto, and the two were thoroughly mixed with stirring for 30 minutes. After that, the mixture was centrifuged, washed multiple times with deionized water, and then dried in a heated environment at 60°C for 12 hours (step S15).

[0040] <Material evaluation of photocatalyst 1> The structure of photocatalyst 1 was examined by XRD (X-ray diffraction), and the results are shown in Figure 1. The XRD device used was X'Pert PRO (manufactured by PANalytical). It can be seen from Figure 1 that ZnO / TiO2(4 / 1) supported with Au particles has ZnO and anatase type TiO2. For reference, Figure 1 also shows the X-ray diffraction data of ZnO / TiO2(4 / 1) and ZnTi-LDHs before supporting Au particles.

[0041] The amount of Au nanoparticles supported was measured by inductively coupled optical emission spectroscopy (ICP-OES), and the result was 1.05% by weight. The ICP-OES device used was Ultima2 (manufactured by HORIBA Jobin Yvon). The results of investigating the particle size of the Au microparticles are shown in Figure 2. The particle size was mostly between 2.0 nm and 5.0 nm, with the majority being between 2.3 nm and 3.8 nm.

[0042] The results of measuring Photocatalyst 1 with a TEM (Transmission Electron Microscope) are shown in Figure 3, the results of measuring it with a HRTEM (High-resolution TEM) are shown in Figure 4, and the results of measuring it with a STEM (Scanning TEM) are shown in Figure 5. Here, the HRTEM device used was a Talos F200S (manufactured by FET), and the STEM device used was a Titan 80-300 (manufactured by FET). It can be seen that ZnO and TiO2 are dispersed in particulate form without any significant bias, and Au is in the form of fine particles that are supported on the ZnO / TiO2 with high dispersion. In addition, the lattice spacings are 0.248 nm for ZnO(101), 0.352 nm for TiO2(101), and 0.235 nm for Au(111), respectively, and clear junctions are observed between the ZnO and TiO2 particles, indicating that heterojunctions have occurred between the ZnO and TiO2 particles. This is thought to be the factor that produces the nanocomposite effect described below.

[0043] The results of analyzing Photocatalyst 1 by EDX (Energy dispersive X-ray spectroscopy) are shown in Figure 6. The elements Zn, O, Ti, and Au were observed, and it was found that they were uniformly dispersed.

[0044] <Photocatalytic ethane production characteristics> Next, the activity of the photocatalyst 1 was evaluated by the method described below. 20 mg of photocatalyst 1 was evenly spread on the bottom surface of a cylindrical reactor with a diameter of 28 mm, and a methane-air mixed gas (CH4 / air ratio = 69; CH4 / oxygen ratio = 345) was passed through it at a flow rate of 70 mL / min. Then, using a 300W Xe lamp (manufactured by Eagle Engineering Co., Ltd.) that emits light with a spectrum similar to that of sunlight and an optical filter (manufactured by HOYA), light with wavelengths between 300nm and 500nm was irradiated at 500mW / cm. 2 The generated gas was measured using a gas chromatograph (GC-FID, Shimadzu Corporation). As a result, the catalyst yield was 5020 μmol h -1 g -1 Ethane is produced at a high rate of 225 μmol h -1 g -1 propane, 278 μmol h -1 g -1 Carbon dioxide production was observed. The results are shown in Table 1. It was found that the production ratio of ethane was high, at approximately 90%.

[0045] [Table 1]

[0046] Example 2 In Example 2, the effect of supporting Au fine particles on photocatalyst 1 was examined. First, the main catalyst, ZnO / TiO2 (4 / 1), was prepared in the same manner as in Example 1, and the metal precursor HAuCl4 was replaced with a precursor containing Ag, Pd, Pt, Cu, Ni, and Ru metals to prepare a photocatalyst through the same process as in Example 1. Specifically, AgNo3, Na2PdCl4, H2PtCl6, Cu(NO3), Ni(NO3), and RuCl3 were used as metal precursors. Here, the amount of each metal supported was adjusted to 1.0 wt%.

[0047] The results of investigating the amount of ethane produced under the same conditions as in Example 1 are shown in Figure 9, the results of investigating the ethane production ratio are shown in Figure 10, and the numerical data are shown in the above-mentioned Table 1. In addition, these figures and tables also include data when no metal is supported. As a result, it was found that by supporting 1 wt% Au nanoparticles, the amount of ethane produced was about one order of magnitude higher than when other metals were supported, and the ethane production ratio was also by far the highest at about 90%. The second highest ethane production ratio after Au nanoparticle support was achieved when Ag nanoparticles were supported, but even in this case the ethane production ratio remained at 35%. When Pt particles were supported, the amount of ethane generated was 0 μmol h -1 g -1 The amount of CO2 produced was 7641 μmol h -1 g -1 The Pt nanoparticle co-catalyst promotes the oxidation of methane to produce CO2, but its oxidizing power is too strong to be suitable for the methane coupling reaction. In addition, in the case of the main catalyst ZnO / TiO2 (4 / 1) without metal atoms, the amount of ethane produced was 0 μmol h -1 g -1 However, it did not function as a photocatalyst for ethane production. It was demonstrated that the support of the co-catalyst by Au nanoparticles is essential for ethane production.

[0048] Next, the amounts of both HAuCl4 and NaBH4 aqueous solutions were adjusted to prepare photocatalysts with Au nanoparticle loadings of 0.1, 0.5, 1.0, and 2.0 wt%, and the dependence of the ethane production amount and ethane production ratio on the amount of Au nanoparticle loading was investigated. Here, the photocatalyst manufacturing method, except for the amounts of HAuCl4 and NaBH4, conformed to Example 1, and the evaluation method for the ethane production amount and production ratio also conformed to Example 1. The results, including the case where no Au fine particles were supported, are shown in FIG. 11 and Table 2.

[0049] [Table 2]

[0050] When the Au particles were loaded at 0.1 wt% or more, a high ethane generation ratio of 86% or more was obtained. In the range of 0.1 wt% to 1.0 wt% Au particles, the amount of ethane generated increased almost linearly with the loading amount, and the amount of ethane generated was about 5000 μmol g -1 h -1 It can be seen that the generation amount is saturated at a high level.

[0051] Example 3 In Example 3, the effect of making the main catalyst ZnO / TiO2 (4 / 1) into a nanocomposite was investigated. For comparison, ZnO and TiO2 were prepared and blended at a molar ratio of 4 / 1 to prepare a blended main catalyst ZnO / TiO2 (4 / 1).Then, photocatalyst B1 (mixed) was prepared, which is a blended main catalyst with 1 wt% Au supported, in accordance with Example 1 except for the blended main catalyst. The amount of ethane produced was evaluated by the method shown in Example 1, and the results are shown in FIG.

[0052] [Table 3]

[0053] In the case of photocatalyst 1, which used a nanocomposite as the main catalyst, the amount of ethane produced was 5020 μmol h -1 g -1 whereas, in the case of the blended photocatalyst B1, it was 2493 μmol h -1 g -1 This is thought to be because the heterojunction of ZnO and TiO2 in the nanocomposite increased the amount of ethane produced.

[0054] Example 4 In Example 4, the dependence of ethane production on the molar ratio of ZnO and TiO2 in the main catalyst with a nanocomposite structure was investigated. There, different molar ratios of Zn 2+ / Ti 4+ ZnO, ZnO / TiO2 (8 / 1), ZnO / TiO2 (4 / 1), ZnO / TiO2 (2 / 1), ZnO / TiO2 (1 / 1), ZnO / TiO2 (1 / 2) and TiO2 were prepared using the ethane ratio (1:0, 8:1, 2:1, 1:1, 1:2 and 0:1), and the amount of ethane produced was evaluated when 1% by weight of Au particles was supported on each main catalyst according to the method of Example 1. The results are shown in Figure 13. Various numerical data such as the ethane production ratio are summarized in Table 4.

[0055] [Table 4]

[0056] As a result, all samples had a concentration of 2000 μmol h -1 g -1 The amount of ethane produced was 2400 μmol h -1 g -1 The ethane production amount and ethane production ratio of 80% or more were both achieved. A high ethane production ratio is practically important for the separation and utilization of ethane. Furthermore, when the molar ratio of ZnO to TiO2 is 0.5 to 4, the ethane production rate was 4000 μmol h -1 g-1 Both a high ethane production rate and an ethane production ratio of over 80% were achieved.

[0057] Example 5 In Example 5, the dependence of the amount and ratio of ethane produced on the mixture gas ratio of methane and oxygen was evaluated. Here, pure air was used as the oxygen-containing gas. Therefore, the amount of oxygen was 20% of the amount of air introduced. Photocatalyst 1 of Example 1 was used as the photocatalyst. The ethane production method was also in accordance with Example 1, and the evaluation was performed by adjusting the flow rates of the methane gas and dry air introduced. The flow rate ratio can be considered to correspond to the molar ratio. The results are shown in Figure 14 and Table 5.

[0058] [Table 5]

[0059] As a result, it is found that the ethane production ratio increases monotonically as the methane ratio CH4 / O2 increases. The ethane production rate is 2950 μmol h when the methane ratio is 2. -1 g -1 As the methane ratio increases from 2 to 10, the amount of ethane produced increases linearly in a semi-logarithmic manner. When the methane ratio exceeds 10, at least up to 345, the amount of ethane produced is about 5000 μmol h -1 g -1 It can be seen that it takes a constant value of . As shown in Table 5, a small amount of ethane is produced from methane gas alone, but its activity is about two orders of magnitude lower.

[0060] Example 6 In Example 6, the effect of using simulated sunlight was evaluated. In this experiment, the light source was changed from a combination of a xenon lamp and an optical filter to an AM1.5G solar simulator, and photocatalyst 1 was evaluated in the same manner as in Example 1. The result was 230 μmol h -1 g-1 Ethane is produced at a rate of 9 μmol h -1 g -1 propane, 14 μmol h -1 g -1 Carbon dioxide was produced (Table 6). Because the amount of light was less than when irradiated with a xenon lamp, the activity decreased, but it was confirmed that about 90% of the products were produced as ethane.

[0061] [Table 6]

[0062] Example 7 In Example 7, the effects of the presence or absence of light irradiation were confirmed. In this experiment, light irradiation was not performed, and the mixture was heated to 150°C in the dark, and the experiment was conducted in accordance with Example 1. As a result, no products of ethane, propane, or carbon dioxide were confirmed (Table 6). In other words, it became clear that light irradiation is essential for the methane coupling ethane production reaction, and that photocatalytic reaction is important for this coupling reaction. [Industrial Applicability]

[0063] As described above, the present invention enables the safe and efficient production of ethane from methane gas. Ethane is one of the fundamental substances that support the chemical industry, and we believe that this will greatly contribute to the industry. Furthermore, the photocatalyst of the present invention is a key component in the production of ethane, and is believed to make a great contribution to the industry. [Explanation of symbols]

[0064] 11: Housing 12: Photocatalyst 13: Window 14:Light 15: Gas inlet 16: Methane gas 17: Valve 18: Gas inlet 19: Oxygen-containing gas (air) 20: Valve 21: Gas outlet 22: Ethane gas 23: Valve 101: Ethane production unit

Claims

1. Zinc oxide (ZnO) and titanium oxide (TiO 2 ) a semiconductor made of a nanocomposite, and gold particles (Au particles) supported on the semiconductor. Photocatalyst that produces ethane from methane.

2. The TiO 2 The photocatalyst according to claim 1 , wherein the molar ratio of ZnO to ZnO is 0.5 or more and 8 or less.

3. The TiO 2 The photocatalyst according to claim 1 , wherein the molar ratio of ZnO to ZnO is 0.5 or more and 4 or less.

4. 4. The photocatalyst according to claim 1, wherein a ratio of said Au fine particles to said photocatalyst is 0.1% by weight or more and 2.0% by weight or less.

5. 4. The photocatalyst according to claim 1, wherein a ratio of said Au fine particles to said photocatalyst is 1.0% by weight or more and 2.0% by weight or less.

6. The photocatalyst according to claim 1 , wherein the Au fine particles have a particle diameter of 2 nm or more and 5 nm or less.

7. The photocatalyst according to claim 1 , wherein the Au fine particles have a particle diameter of 2.3 nm or more and 3.8 nm or less.

8. Providing a layered hydroxide containing ZnTi ions; The layered hydroxide is heat-treated in the presence of oxygen to form ZnO and TiO 2 and preparing a composite comprising: The composite was suspended in an aqueous solution to form ZnO and TiO 2 preparing an aqueous suspension comprising: The suspension was added to HAuCl 4 Add an aqueous solution of HAuCl 4 preparing an additive aqueous solution; The HAuCl 4A method for producing a photocatalyst for producing ethane from methane, comprising the steps of adding a reducing agent to an additive aqueous solution, and then drying the solution to produce a photocatalyst.

9. The method for producing a photocatalyst according to claim 8, wherein the temperature of the heat treatment is 200°C or more and 800°C or less.

10. The reducing agent is NaBH 4 The method for producing a photocatalyst according to claim 8 or 9, wherein the photocatalyst is an aqueous solution.

Citation Information

Patent Citations

  • Method for cleaning metal carrying catalyst

    JP2005219030A

  • photocatalyst

    JP2005279545A

  • Composite type particulate photocatalyst, method for manufacturing the same and coating agent and photocatalytically-active member using the same

    JP2007144403A

  • Reactor and production method of carbohydrate

    JP2019127641A

  • Catalyst and process for producing hydrocarbon

    JP2020028821A