Circular polarizing plate, organic electroluminescence display device

The circularly polarizing plate with optimized twist angles and refractive index anisotropy products in optically anisotropic layers addresses the issue of color change and reflectance in organic electroluminescent display devices, improving image quality from oblique views.

JP7578692B2Active Publication Date: 2024-11-06FUJIFILM CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022531969
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-22
Filing Date
2021-06-21
Publication Date
2024-11-06
Estimated Expiration
2041-06-21

AI Technical Summary

Technical Problem

Existing circularly polarizing plates for organic electroluminescent display devices do not adequately reduce color change and reflectance when viewed from oblique directions, failing to meet the requirements for improved image quality.

Method used

A circularly polarizing plate configuration with a polarizer and optically anisotropic layers formed using reverse wavelength dispersion liquid crystal compounds, where the molecular axes of the liquid crystal compounds are horizontally aligned to the layer surfaces, and specific twist angles and refractive index anisotropy products are optimized to minimize color change and reflectance.

Benefits of technology

The proposed configuration significantly reduces color change and reflectance when viewed from oblique directions, enhancing the image quality of organic electroluminescent display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578692000014
    Figure 0007578692000014
  • Figure 0007578692000015
    Figure 0007578692000015
  • Figure 0007578692000016
    Figure 0007578692000016
Patent Text Reader

Abstract

The present invention provides a circularly polarizing plate and an organic electroluminescence display device, wherein, when the display device obtained by disposing the circularly polarizing plate on a display element is viewed from an oblique direction while the orientation thereof is being changed, the display device shows little change in color tone, and has low reflectance. This circular polarizing plate comprises a polarizer and an optically anisotropic layer. The optically anisotropic layer is obtained by immobilizing a reverse wavelength dispersive liquid crystal compound that is twisted aligned with a thickness direction as a helical axis, the molecular axis of the liquid crystal compound in the optically anisotropic layer is horizontal to the surface of the optically anisotropic layer, and the twist angle of the twisted aligned liquid crystal compound is 15-360°.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a circular polarizing plate and an organic electroluminescence display device. [Background technology]

[0002] 2. Description of the Related Art Optically anisotropic layers having refractive index anisotropy are used in various applications, such as antireflection films for display devices and optical compensation films for liquid crystal display devices. Patent Document 1 discloses a circular polarizing plate having an optically anisotropic layer formed using a liquid crystal compound with reverse wavelength dispersion. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-111257 A Summary of the Invention [Problem to be solved by the invention]

[0004] Meanwhile, in recent years, in display devices typified by organic electroluminescence (EL) display devices, in order to further improve image quality, it is desirable for there to be little change in color when the display device is viewed from an oblique direction while changing the orientation. It is also desirable that the reflectance be low. More specifically, it is also desirable that the average reflectance, which is the average value of the reflectance in each direction when viewed from an oblique direction and in different directions, be low.

[0005] The present inventors produced the circular polarizing plate disclosed in Patent Document 1, attached it to a display element, and evaluated its performance, and found that it did not fully satisfy the above-mentioned demands.

[0006] In view of the above-mentioned circumstances, an object of the present invention is to provide a circular polarizing plate which, when placed on a display element, causes little change in color and has a low reflectance when the resulting display device is viewed from an oblique direction while changing the orientation. Another object of the present invention is to provide an organic electroluminescence display device. [Means for solving the problem]

[0007] As a result of extensive investigation into the problems of the conventional techniques, the present inventors have found that the above-mentioned problems can be solved by the following configuration.

[0008] (1) A circular polarizing plate having a polarizer and an optically anisotropic layer, The optically anisotropic layer is a layer in which a liquid crystal compound with reverse wavelength dispersion is fixed and twisted and aligned with a helical axis in the thickness direction. the molecular axis of the liquid crystal compound in the optically anisotropic layer is parallel to the surface of the optically anisotropic layer, A circular polarizing plate in which the twist angle of the twisted liquid crystal compound is 15 to 360°. (2) The optically anisotropic layer formed by using a liquid crystal compound is the above-mentioned optically anisotropic layer alone, The twist angle is within the range of 64±20°, The circularly polarizing plate according to (1), wherein the product Δnd of the refractive index anisotropy Δn of the optically anisotropic layer measured at a wavelength of 550 nm and the thickness d of the optically anisotropic layer is 160 to 240 nm. (3) A polarizer, a second optically anisotropic layer, and a first optically anisotropic layer in this order; the first optically anisotropic layer is a layer in which a liquid crystal compound having reverse wavelength dispersion is fixed and is twisted and aligned with a helical axis in the thickness direction; the molecular axis of the liquid crystal compound in the first optically anisotropic layer is parallel to the surface of the first optically anisotropic layer; the second optically anisotropic layer is a layer in which a liquid crystal compound having a reverse wavelength dispersion property is fixed in a homogeneously aligned state, the twist angle in the first optically anisotropic layer is within the range of 85±20°; an in-plane slow axis of the first optically anisotropic layer on the second optically anisotropic layer side is parallel to an in-plane slow axis of the second optically anisotropic layer on the first optically anisotropic layer side; the value of the product Δn1d1 of the refractive index anisotropy Δn1 of the first optically anisotropic layer measured at a wavelength of 550 nm and the thickness d1 of the first optically anisotropic layer satisfies the relationship of formula (1) described below, The circularly polarizing plate according to (1), wherein the product Δn2d2 of the refractive index anisotropy Δn2 of the second optically anisotropic layer measured at a wavelength of 550 nm and the thickness d2 of the second optically anisotropic layer satisfies the relationship of formula (2) described below. (4) A polarizer, a fourth optically anisotropic layer, and a third optically anisotropic layer in this order; the third optically anisotropic layer is a layer in which a liquid crystal compound having reverse wavelength dispersion is fixed and is twisted and aligned with a helical axis in the thickness direction; the molecular axis of the liquid crystal compound in the third optically anisotropic layer is parallel to the surface of the third optically anisotropic layer; the fourth optically anisotropic layer is a layer in which a liquid crystal compound having reverse wavelength dispersion is fixed and is twisted and aligned with a helical axis in the thickness direction; the molecular axis of the liquid crystal compound in the fourth optically anisotropic layer is parallel to the surface of the fourth optically anisotropic layer; the twist direction of the liquid crystal compound in the third optically anisotropic layer is the same as the twist direction of the liquid crystal compound in the fourth optically anisotropic layer; the twist angle of the liquid crystal compound in the fourth optically anisotropic layer is within the range of 26.5±10.0°; the twist angle of the liquid crystal compound in the third optically anisotropic layer is within the range of 78.6±10.0°; an in-plane slow axis of the third optically anisotropic layer on the surface facing the fourth optically anisotropic layer is parallel to an in-plane slow axis of the fourth optically anisotropic layer on the surface facing the third optically anisotropic layer; The circularly polarizing plate described in (1), in which the product Δn3d3 of the refractive index anisotropy Δn3 of the third optical anisotropic layer measured at a wavelength of 550 nm and the thickness d3 of the optical anisotropic layer, and the product Δn4d4 of the refractive index anisotropy Δn4 of the fourth optical anisotropic layer measured at a wavelength of 550 nm and the thickness d4 of the fourth optical anisotropic layer respectively satisfy the following equations (3) and (4). (5) The circular polarizing plate according to any one of (1) to (4), wherein the liquid crystal compound having reverse wavelength dispersion is a rod-shaped liquid crystal compound having reverse wavelength dispersion. (6) An organic electroluminescence display device having the circular polarizing plate according to any one of (1) to (5). Effect of the Invention

[0009] According to the present invention, it is possible to provide a circular polarizing plate which, when placed on a display element and the resulting display device is viewed from an oblique direction while changing the orientation, undergoes little change in color and has a low reflectance. The present invention also provides an organic electroluminescence display device. [Brief description of the drawings]

[0010] [Figure 1] 1 is an example of a schematic cross-sectional view of a first embodiment of a circular polarizing plate of the present invention. [Diagram 2] FIG. 2 is an example of a schematic cross-sectional view of a second embodiment of the circular polarizing plate of the present invention. [Diagram 3] FIG. 1 shows the relationship between the absorption axis of a polarizer 10 and the in-plane slow axes of a first optically anisotropic layer 14 and a second optically anisotropic layer 16 in one aspect of the second embodiment of the circular polarizing plate of the present invention. [Figure 4] 4 is a schematic diagram showing the relationship between the absorption axis of a polarizer 10 and the angles between the in-plane slow axes of a first optically anisotropic layer 14 and a second optically anisotropic layer 16 when observed from the direction of the arrow in FIG. [Diagram 5] FIG. 1 shows the relationship between the absorption axis of a polarizer 10 and the in-plane slow axes of a first optically anisotropic layer 14 and a second optically anisotropic layer 16 in one aspect of the second embodiment of the circular polarizing plate of the present invention. [Figure 6] 6 is a schematic diagram showing the relationship between the absorption axis of a polarizer 10 and the angles between the in-plane slow axes of a first optically anisotropic layer 14 and a second optically anisotropic layer 16 when observed from the direction of the arrow in FIG. 5. FIG. [Figure 7] FIG. 2 is a cross-sectional view of a composition layer for explaining step 1. [Figure 8] FIG. 11 is a cross-sectional view of a composition layer for explaining step 2. [Figure 9]FIG. 2 is a schematic diagram of a graph plotting the relationship between the helical twisting power (HTP) (μm−1)×concentration (mass%) and the light irradiation dose (mJ / cm2) for each of chiral agents A and B. [Figure 10] FIG. 1 is a schematic diagram of a graph plotting the relationship between the weighted average helical twisting power (μm−1) and the light irradiation dose (mJ / cm2) in a system in which chiral agent A and chiral agent B are used in combination. [Figure 11] FIG. 11 is a cross-sectional view of a composition layer for illustrating a case where step 5 is carried out. [Figure 12] FIG. 2 is an example of a schematic cross-sectional view of a third embodiment of a circular polarizing plate of the present invention. [Figure 13] FIG. 1 shows the relationship between the absorption axis of a polarizer 10 and the in-plane slow axes of a third optically anisotropic layer 22 and a fourth optically anisotropic layer 24 in one aspect of the third embodiment of the circular polarizing plate of the present invention. [Figure 14] 14 is a schematic diagram showing the relationship between the absorption axis of a polarizer 10 and the angle between the absorption axis of each of the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24 when observed from the direction of the arrow in FIG. [Figure 15] FIG. 1 shows the relationship between the absorption axis of a polarizer 10 and the in-plane slow axes of a third optically anisotropic layer 22 and a fourth optically anisotropic layer 24 in one aspect of the third embodiment of the circular polarizing plate of the present invention. [Figure 16] 16 is a schematic diagram showing the relationship between the absorption axis of a polarizer 10 and the angle between the absorption axis of each of the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24 when observed from the direction of the arrow in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. In this specification, a numerical range expressed using "to" means a range including the numerical values ​​before and after "to" as the lower and upper limits. First, the terms used in this specification will be described.

[0012] The in-plane slow axis is defined at 550 nm unless otherwise specified.

[0013] In the present invention, Re(λ) and Rth(λ) respectively represent the in-plane retardation and the retardation in the thickness direction at a wavelength λ, which is set to 550 nm unless otherwise specified. In the present invention, Re(λ) and Rth(λ) are values ​​measured at a wavelength λ using an AxoScan (manufactured by Axometrics). By inputting the average refractive index ((nx+ny+nz) / 3) and the film thickness (d(μm)) into AxoScan, Slow axis direction (°) Re(λ)=R0(λ) Rth(λ)=((nx+ny) / 2-nz)×d is calculated. Note that R0(λ) is displayed as a numerical value calculated by AxoScan, but it means Re(λ).

[0014] In this specification, the refractive indices nx, ny, and nz are measured using an Abbe refractometer (NAR-4T, manufactured by Atago Co., Ltd.) and a sodium lamp (λ=589 nm) as a light source. In addition, when measuring wavelength dependency, it can be measured using a multi-wavelength Abbe refractometer DR-M2 (manufactured by Atago Co., Ltd.) in combination with an interference filter. In addition, values ​​from the Polymer Handbook (JOHN WILEY & SONS, INC.) and catalogs of various optical films can be used. The average refractive index values ​​of major optical films are shown below as examples: cellulose acylate (1.48), cycloolefin polymer (1.52), polycarbonate (1.59), polymethyl methacrylate (1.49), and polystyrene (1.59).

[0015] In this specification, "light" refers to actinic rays or radiation, such as the emission line spectrum of a mercury lamp, far ultraviolet rays represented by excimer lasers, extreme ultraviolet rays (EUV light: Extreme Ultraviolet), X-rays, ultraviolet rays, and electron beams (EB).

[0016] In this specification, "visible light" refers to light having a wavelength of 380 to 780 nm. In addition, in this specification, unless otherwise specified, the measurement wavelength is 550 nm. In this specification, the angular relationship (e.g., "perpendicular", "parallel", etc.) is assumed to include the range of error permitted in the technical field to which the present invention pertains. Specifically, this means that the angle is within the range of ±10° from the exact angle, and the error from the exact angle is preferably within the range of ±5°, and more preferably within the range of ±3° or less.

[0017] The circular polarizing plate of the present invention has a polarizer and an optically anisotropic layer. The optically anisotropic layer is a layer in which a liquid crystal compound with reverse wavelength dispersion is fixed and twisted and oriented with the thickness direction as a helical axis, the molecular axis of the liquid crystal compound in the optically anisotropic layer is parallel to the surface of the optically anisotropic layer, and the twist angle of the twisted and oriented liquid crystal compound is 15 to 360°. The term "horizontal" means that the average molecular axis of the liquid crystal compound in the optically anisotropic layer forms an inclination angle of less than 20° with the surface of the optically anisotropic layer. The inclination angle of the average molecular axis of the liquid crystal compound with the surface of the optically anisotropic layer is measured using an AxoScan (polarimeter) device manufactured by Axometrics and the device analysis software of the same company. The present inventors have found that the effects of the present invention can be obtained by using an optically anisotropic layer in which a liquid crystal compound having reverse wavelength dispersion is fixed and in which the twist angle is within a predetermined range.

[0018] Specific embodiments of the circularly polarizing plate of the present invention will be described in detail below.

[0019] <First embodiment> A first embodiment of the circular polarizer of the present invention will be described with reference to the drawings. Fig. 1 shows a schematic cross-sectional view of the first embodiment of the circular polarizer of the present invention. The circular polarizing plate 100A has a polarizer 10 and an optically anisotropic layer 12. The optically anisotropic layer 12 is a layer formed by using a rod-shaped liquid crystal compound LC. The optically anisotropic layer 12 is a layer formed by fixing a rod-shaped liquid crystal compound LC that is twisted and aligned with the thickness direction as a helical axis, and the molecular axis of the rod-shaped liquid crystal compound LC in the optically anisotropic layer 12 is horizontal to the surface of the optically anisotropic layer 12. That is, the rod-shaped liquid crystal compound LC shown in the optically anisotropic layer 12 is twisted and aligned in the optically anisotropic layer 12. In FIG. 1, a rod-shaped liquid crystal compound is used to form the optically anisotropic layer 12, but the liquid crystal compound is not limited to a rod-shaped liquid crystal compound as described later. In the circular polarizing plate 100A, the optically anisotropic layer formed using a liquid crystal compound only includes the optically anisotropic layer 12. That is, in the circular polarizing plate 100A, the optically anisotropic layer formed using a liquid crystal compound has a single-layer structure, and only the optically anisotropic layer 12, which is a single layer, is included as the optically anisotropic layer formed using a liquid crystal compound. Each layer will be described in detail below.

[0020] (Polarizer 10) The polarizer 10 (linear polarizer) may be any member having a function of converting natural light into a specific linearly polarized light, and an example of such a member is an absorptive polarizer. There is no particular limitation on the type of polarizer 10, and any commonly used polarizer can be used, such as an iodine-based polarizer, a dye-based polarizer using a dichroic dye, and a polyene-based polarizer. Iodine-based polarizers and dye-based polarizers are generally produced by adsorbing iodine or a dichroic dye to polyvinyl alcohol and stretching it. A protective film may be disposed on one or both surfaces of the polarizer 10.

[0021] (Optical anisotropic layer 12) The optically anisotropic layer 12 is a layer in which liquid crystal compounds are fixed and twisted with the thickness direction as the helical axis, and the molecular axis of the liquid crystal compounds in the optically anisotropic layer 12 is parallel to the surface of the optically anisotropic layer 12 . In this specification, a liquid crystal compound with reverse wavelength dispersion refers to a liquid crystal compound that, when an optically anisotropic layer produced using only this compound has an in-plane retardation (Re) value measured at a specific wavelength (visible light range), has a Re value that is the same or higher as the measured wavelength increases. In this specification, the molecular axis being parallel to the surface of the optically anisotropic layer means that the average molecular axis of the liquid crystal compound forms an inclination angle with the surface of the optically anisotropic layer of less than 20°, as described above. The method for measuring the inclination angle is as described above. In addition, in this specification, the molecular axis means the long axis (molecular long axis) when the liquid crystal compound is a rod-shaped liquid crystal compound, and means the axis parallel to the normal direction to the discotic surface of the discotic liquid crystal compound when the liquid crystal compound is a discotic liquid crystal compound.

[0022] The optically anisotropic layer 12 is preferably a layer in which a chiral nematic phase having a so-called helical structure is fixed. In other words, the optically anisotropic layer 12 is preferably a layer in which a liquid crystal compound is fixed, the molecular axis of which is horizontally aligned and twisted with the thickness direction as the helical axis. When forming the above phase, it is preferable to use a mixture of a liquid crystal compound exhibiting a nematic liquid crystal phase and a chiral agent described later. In this specification, the "fixed" state refers to a state in which the alignment of the liquid crystal compound is maintained. Specifically, it is preferable that the layer has no fluidity in a temperature range of usually 0 to 50° C., or under more severe conditions, −30 to 70° C., and that the alignment state is not changed by an external field or external force, and the fixed alignment state can be stably maintained.

[0023] The twist angle of the liquid crystal compound in the optically anisotropic layer 12 (the twist angle of the alignment direction of the rod-like liquid crystal compound LC) is preferably within a range of 64±20°. That is, the twist angle of the liquid crystal compound is preferably 44 to 84°. In particular, it is preferably 54 to 74°, and more preferably 59 to 69°, in terms of less change in color and / or lower reflectance when a circularly polarizing plate is placed on a display element and the resulting display device is viewed from an oblique direction while changing the orientation (hereinafter, also simply referred to as "the point where the effect of the present invention is better"). The liquid crystal compound is twisted around the thickness direction of the optically anisotropic layer 12. Accordingly, the alignment direction (in-plane slow axis direction) of the liquid crystal compound varies depending on the position in the thickness direction of the optically anisotropic layer 12. In addition, there are two kinds of twist directions, which may be right-handed or left-handed. In Fig. 1, right-handed twist means that when observed from the polarizer 10 toward the optically anisotropic layer 12, the in-plane slow axis of the optically anisotropic layer 12 on the opposite side to the polarizer 10 side is positioned clockwise with respect to the in-plane slow axis of the optically anisotropic layer 12 on the polarizer 10 side, which serves as the reference axis.

[0024] The torsion angle is measured using an AxoScan (polarimeter) device manufactured by Axometrics Inc. and the device analysis software of the same company.

[0025] The value of the product Δnd of the refractive index anisotropy Δn of the optically anisotropic layer 12 measured at a wavelength of 550 nm and the thickness d of the optically anisotropic layer 12 is preferably 160 to 240 nm, more preferably 170 to 230 nm, even more preferably 180 to 220 nm, and particularly preferably 190 to 210 nm, in order to obtain better effects of the present invention. The above Δnd is measured using an AxoScan (polarimeter) device manufactured by Axometrics Inc. and the device analysis software of the same company, in the same manner as in the measurement of the torsion angle.

[0026] The thickness of the optically anisotropic layer 12 is not particularly limited, and from the viewpoint of thinning, it is preferably 10 μm or less, more preferably 0.5 to 8.0 μm, and even more preferably 0.5 to 6.0 μm. In this specification, the thickness of the optically anisotropic layer refers to the average thickness of the optically anisotropic layer, which is determined by measuring the thicknesses of the optically anisotropic layer at any five or more positions and calculating the arithmetic average of the measured values.

[0027] It is preferable that the in-plane slow axis of the surface of the optically anisotropic layer 12 facing the polarizer 10 is parallel to the absorption axis of the polarizer 10. The definition of parallel is as described above. That is, the angle between the in-plane slow axis of the surface of the optically anisotropic layer 12 facing the polarizer 10 and the absorption axis of the polarizer 10 is preferably within 10° (0 to 10°). In particular, in terms of better effects of the present invention, it is more preferable that the angle between the in-plane slow axis of the surface of the optically anisotropic layer 12 facing the polarizer 10 and the absorption axis of the polarizer 10 is less than 5° (0° or more and less than 5°).

[0028] As described above, in FIG. 1, a rod-shaped liquid crystal compound is used to form the optically anisotropic layer 12, but the present invention is not limited to this embodiment. Generally, liquid crystal compounds can be classified into rod-shaped type (rod-shaped liquid crystal compounds) and discotic type (disctic liquid crystal compounds) based on their shape. Furthermore, there are low molecular type and polymer type. Polymer generally refers to a compound with a degree of polymerization of 100 or more (Polymer Physics, Phase Transition Dynamics, by Masao Doi, page 2, Iwanami Shoten, 1992). In the present invention, any liquid crystal compound can be used. In addition, in the present invention, two or more rod-shaped liquid crystal compounds, two or more discotic liquid crystal compounds, or a mixture of rod-shaped and discotic liquid crystal compounds may be used. Examples of rod-shaped liquid crystal compounds include those described in claim 1 of JP-T-11-513019 and paragraphs

[0026] to

[0098] of JP-A-2005-289980. Examples of discotic liquid crystal compounds include those described in paragraphs

[0020] to

[0067] of JP-A-2007-108732 and paragraphs

[0013] to

[0108] of JP-A-2010-244038.

[0029] It is more preferable to form the optically anisotropic layer 12 using a liquid crystal compound having a polymerizable group and reverse wavelength dispersion (hereinafter simply referred to as a "polymerizable liquid crystal compound"), since this can reduce changes in temperature or humidity. That is, the optically anisotropic layer 12 is preferably a layer formed by fixing a liquid crystal compound having a reverse wavelength dispersion property and a polymerizable group by polymerization or the like. The type of polymerizable group is not particularly limited, and is preferably a functional group capable of an addition polymerization reaction, more preferably a polymerizable ethylenically unsaturated group or a ring-polymerizable group, further preferably a (meth)acryloyl group, a vinyl group, a styryl group, or an allyl group, and particularly preferably a (meth)acryloyl group.

[0030] The polymerizable liquid crystal compound is preferably a polymerizable liquid crystal compound represented by the following formula (I). L1-G1-D1-Ar-D2-G2-L2...(I)

[0031] In formula (I), D1 and D2 each independently represent a single bond, -O-, -CO-, -CO-O-, -C(=S)O-, -CR 1 R 2 -, -CR 1 R 2 -CR 3 R 4 -, -O-CR 1 R 2 -, -CR 1 R 2 -O-CR 3 R 4 -,-CO-O-CR 1 R 2 -, -O-CO-CR 1 R 2 -, -CR 1 R 2 -CR 3 R 4 -O-CO-, -CR 1 R 2 -O-CO-CR 3 R 4 -, -CR 1 R 2 -CO-O-CR 3R 4 -, -NR 1 -CR 2 R 3 -, or -CO-NR 1 - represents. R 1 , R 2 , R 3 and R 4 R each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 4 carbon atoms. 1 , R 2 , R 3 and R 4 If there are multiple of each, multiple R 1 , multiple R 2 , multiple R 3 and multiple R 4 may be the same or different from each other. G1 and G2 each independently represent a divalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, a group formed by linking a plurality of the above-mentioned alicyclic hydrocarbon groups, an aromatic hydrocarbon group, or a group formed by linking a plurality of the above-mentioned aromatic hydrocarbon groups, and a methylene group contained in the above-mentioned alicyclic hydrocarbon group may be substituted with -O-, -S-, or NH-. The group formed by linking a plurality of the alicyclic hydrocarbon groups refers to a group formed by linking divalent alicyclic hydrocarbon groups having 5 to 8 carbon atoms with each other via a single bond. In addition, the group formed by linking a plurality of the aromatic hydrocarbon groups refers to a group formed by linking aromatic hydrocarbon groups with each other via a single bond. L1 and L2 each independently represent a monovalent organic group, and at least one selected from the group consisting of L1 and L2 represents a monovalent group having a polymerizable group. Ar represents any aromatic ring selected from the group consisting of groups represented by formulae (Ar-1) to (Ar-7).

[0032] [ka]

[0033] In the above formula (Ar-1), Q 1 represents N or CH, and Q 2is -S-, -O-, or -N(R 7 )-, R 7 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; Y 1 represents an aromatic hydrocarbon group having 6 to 12 carbon atoms or an aromatic heterocyclic group having 3 to 12 carbon atoms, which may have a substituent. R 7 Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, and an n-hexyl group. Y 1 Examples of the aromatic hydrocarbon group having 6 to 12 carbon atoms include aryl groups such as a phenyl group, a 2,6-diethylphenyl group, and a naphthyl group. Y 1 Examples of the aromatic heterocyclic group having 3 to 12 carbon atoms include heteroaryl groups such as a thienyl group, a thiazolyl group, a furyl group, and a pyridyl group. Also, Y 1 Examples of the substituent that may be contained in the group include an alkyl group, an alkoxy group, and a halogen atom. The alkyl group is preferably an alkyl group having 1 to 18 carbon atoms, more preferably an alkyl group having 1 to 8 carbon atoms (e.g., methyl group, ethyl group, propyl group, isopropyl group, n-butyl group, isobutyl group, sec-butyl group, t-butyl group, and cyclohexyl group), still more preferably an alkyl group having 1 to 4 carbon atoms, and particularly preferably a methyl group or an ethyl group. The alkyl group may be linear, branched, or cyclic. The alkoxy group is, for example, preferably an alkoxy group having 1 to 18 carbon atoms, more preferably an alkoxy group having 1 to 8 carbon atoms (for example, a methoxy group, an ethoxy group, an n-butoxy group, and a methoxyethoxy group), still more preferably an alkoxy group having 1 to 4 carbon atoms, and particularly preferably a methoxy group or an ethoxy group. Examples of halogen atoms include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Of these, a fluorine atom or a chlorine atom is preferable.

[0034] In addition, in the above formulas (Ar-1) to (Ar-7), Z 1 , Z 2 and Z 3 each independently represents a hydrogen atom, a monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, a monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms, a monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms, a halogen atom, a cyano group, a nitro group, -OR 8 , -NR 9 R 10 , or -SR 11 R 8 ~R 11 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms; Z 1 and Z 2 may be bonded to each other to form an aromatic ring. As the monovalent aliphatic hydrocarbon group having 1 to 20 carbon atoms, an alkyl group having 1 to 15 carbon atoms is preferable, an alkyl group having 1 to 8 carbon atoms is more preferable, a methyl group, an ethyl group, an isopropyl group, a tert-pentyl group (1,1-dimethylpropyl group), a tert-butyl group, or a 1,1-dimethyl-3,3-dimethyl-butyl group is further preferable, and a methyl group, an ethyl group, or a tert-butyl group is particularly preferable. Examples of the monovalent alicyclic hydrocarbon group having 3 to 20 carbon atoms include monocyclic saturated hydrocarbon groups such as a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a cycloheptyl group, a cyclooctyl group, a cyclodecyl group, a methylcyclohexyl group, and an ethylcyclohexyl group; monocyclic unsaturated hydrocarbon groups such as a cyclobutenyl group, a cyclopentenyl group, a cyclohexenyl group, a cycloheptenyl group, a cyclooctenyl group, a cyclodecenyl group, a cyclopentadienyl group, a cyclohexadienyl group, a cyclooctadienyl group, and a cyclodecadiene group; and monocyclic unsaturated hydrocarbon groups such as a bicyclo[2.2.1]heptyl group, a bicyclo[2.2.2]octyl group, a tricyclo[5.2.1.0]cyclopentyl group, a bicyclo[2.2.2]octyl group, a tricyclo[5.2.1.0]cyclohex ... 2,6 ]decyl group, tricyclo[3.3.1.1 3,7 ]decyl group, tetracyclo[6.2.1.1 3,6 .0 2,7]dodecyl group, and polycyclic saturated hydrocarbon groups such as adamantyl group; and the like. Examples of the monovalent aromatic hydrocarbon group having 6 to 20 carbon atoms include a phenyl group, a 2,6-diethylphenyl group, a naphthyl group, and a biphenyl group, and an aryl group having 6 to 12 carbon atoms (particularly a phenyl group) is preferred. Examples of halogen atoms include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom. Of these, a fluorine atom, a chlorine atom, or a bromine atom is preferable. R 8 ~R 11 Examples of the alkyl group having 1 to 6 carbon atoms include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, and an n-hexyl group.

[0035] In addition, in the above formulas (Ar-2) and (Ar-3), A 1 and A 2 are each independently -O-, -N(R 12 R represents a group selected from the group consisting of -, -S-, and -CO-; 12 represents a hydrogen atom or a substituent. R 12 The substituent represented by the formula (Ar-1) is preferably Y 1 The substituents may be the same as those which may be possessed by the group.

[0036] In addition, in the above formula (Ar-2), X represents a nonmetallic atom of Groups 14 to 16. The nonmetallic atom may have a hydrogen atom or a substituent bonded thereto. Examples of the nonmetallic atom of Groups 14 to 16 represented by X include an oxygen atom, a sulfur atom, a nitrogen atom having a substituent, and a carbon atom having a substituent (*=C-(R)2. * represents a bonding position. R represents a substituent). Examples of the substituent include an alkyl group, an alkoxy group, an alkyl-substituted alkoxy group, a cyclic alkyl group, an aryl group (e.g., a phenyl group and a naphthyl group), a cyano group, an amino group, a nitro group, an alkylcarbonyl group, a sulfo group, and a hydroxyl group.

[0037] In addition, in the above formula (Ar-3), D 4 and D. 5 each independently represents a single bond, -CO-, -O-, -S-, -C(=S)-, or -CR 1a R 2a -, -CR 3a =CR 4a -, -NR 5a -, or a divalent linking group consisting of two or more of these, R 1a ~R 5a each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 4 carbon atoms. Here, examples of the divalent linking group include -CO-, -O-, -CO-O-, -C(=S)O-, -CR 1b R 2b -, -CR 1b R 2b -CR 1b R 2b -, -O-CR 1b R 2b -, -CR 1b R 2b -O-CR 1b R 2b -,-CO-O-CR 1b R 2b -, -O-CO-CR 1b R 2b -, -CR 1b R 2b -O-CO-CR 1b R 2b -, -CR 1b R 2b -CO-O-CR 1b R 2b -, -NR3b -CR 1b R 2b - and -CO-NR 3b - is one of them. 1b , R 2b and R 3b each independently represents a hydrogen atom, a fluorine atom, or an alkyl group having 1 to 4 carbon atoms.

[0038] In addition, in the above formula (Ar-3), SP 1 and S.P. 2 each independently represents a single bond, a linear or branched alkylene group having 1 to 12 carbon atoms, or a divalent linking group in which one or more of -CH2- constituting a linear or branched alkylene group having 1 to 12 carbon atoms is replaced with -O-, -S-, -NH-, -N(Q)-, or -CO-, and Q represents a substituent. 1 The substituents include the same ones as those which may be possessed by the group. Here, examples of preferred linear or branched alkylene groups having 1 to 12 carbon atoms include methylene, ethylene, propylene, butylene, pentylene, hexylene, methylhexylene and heptylene groups.

[0039] In addition, in the above formula (Ar-3), L 3 and L 4 each independently represents a monovalent organic group. Examples of the monovalent organic group include an alkyl group, an aryl group, and a heteroaryl group. The alkyl group may be linear, branched, or cyclic, but is preferably linear. The number of carbon atoms in the alkyl group is preferably 1 to 30, more preferably 1 to 20, and even more preferably 1 to 10. The aryl group may be monocyclic or polycyclic, but is preferably monocyclic. The number of carbon atoms in the aryl group is preferably 6 to 25, and more preferably 6 to 10. The heteroaryl group may be monocyclic or polycyclic. The number of heteroatoms constituting the heteroaryl group is preferably 1 to 3. The heteroatom constituting the heteroaryl group is preferably a nitrogen atom, a sulfur atom, or an oxygen atom. The number of carbon atoms in the heteroaryl group is preferably 6 to 18, and more preferably 6 to 12. The alkyl group, the aryl group, and the heteroaryl group may be unsubstituted or may have a substituent. As the substituent, Y in the above formula (Ar-1) may be used. 1 The substituents may be the same as those which may be possessed by the group.

[0040] In addition, in the above formulas (Ar-4) to (Ar-7), Ax represents an organic group having 2 to 30 carbon atoms and having at least one aromatic ring selected from the group consisting of aromatic hydrocarbon rings and aromatic heterocycles. In the above formulas (Ar-4) to (Ar-7), Ay represents a hydrogen atom, an alkyl group having 1 to 12 carbon atoms which may have a substituent, or an organic group having 2 to 30 carbon atoms and having at least one aromatic ring selected from the group consisting of aromatic hydrocarbon rings and aromatic heterocycles. Here, the aromatic rings in Ax and Ay may have a substituent, and Ax and Ay may be bonded to each other to form a ring. Also, Q 3 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms which may have a substituent. Examples of Ax and Ay include those described in paragraphs

[0039] to

[0095] of Patent Document 2 (WO 2014 / 010325). Also, Q 3Examples of the alkyl group having 1 to 6 carbon atoms represented by the formula (Ar-1) include a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, and an n-hexyl group. 1 The substituents include the same ones as those which may be possessed by the group.

[0041] The definition and preferred range of each substituent of the liquid crystal compound represented by formula (III) are described in JP-A-2012-021068, which is related to compound (A). 1 , D 2 , G 1 , G 2 , L 1 , L 2 , R 4 , R 5 , R 6 , R 7 , X 1 , Y 1 , Q 1 , Q 2 The descriptions for D1, D2, G1, G2, L1, L2, and R are respectively. 1 , R 2 , R 3 , R 4 , Q1, Y1, Z1, and Z2 can be referred to, and the description of A1, A2, and X for the compound represented by general formula (I) described in JP-A-2008-107767 can be referred to, respectively, and the description of Ax, Ay, Q for the compound represented by general formula (I) described in WO 2013 / 018526 can be referred to. 1 The descriptions for Ax, Ay, and Q are 3 For Z3, see Q relating to compound (A) described in JP-A-2012-021068. 1 Please refer to the description below.

[0042] In particular, the organic groups represented by L1 and L2 are preferably groups represented by *-D3-G3-Sp-P3, respectively, where * represents a bonding position. D3 is synonymous with D1. G3 represents a single bond, a divalent aromatic or heterocyclic group having 6 to 12 carbon atoms, a group formed by linking a plurality of the above aromatic or heterocyclic groups, a divalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, or a group formed by linking a plurality of the above alicyclic hydrocarbon groups, and a methylene group contained in the above alicyclic hydrocarbon group is -O-, -S-, or NR 7 -, where R 7 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. The group formed by linking a plurality of the aromatic ring groups or heterocyclic groups refers to a group formed by linking divalent aromatic ring groups or heterocyclic groups having 6 to 12 carbon atoms with each other via a single bond. In addition, the group formed by linking a plurality of the alicyclic hydrocarbon groups refers to a group formed by linking divalent alicyclic hydrocarbon groups having 5 to 8 carbon atoms with each other via a single bond. As G3, a group in which two cyclohexane rings are bonded via a single bond is also preferred. Sp is a single bond, -(CH2) n -, -(CH2) n -O-, -(CH2-O-) n -, -(CH2CH2-O-) m , -O-(CH2) n -, -O-(CH2) n -O-, -O-(CH2-O-) n -, -O-(CH2CH2-O-) m , -C(=O)-O-(CH2) n -, -C(=O)-O-(CH2) n -O-, -C(=O)-O-(CH2-O-) n -, -C(=O)-O-(CH2CH2-O-) m , -C(=O)-N(R 8 )-(CH2) n -, -C(=O)-N(R 8 )-(CH2) n -O-, -C(=O)-N(R 8 )-(CH2-O-) n -, -C(=O)-N(R 8 )-(CH2CH2-O-) m , or -(CH2) n -O-(C=O)-(CH2) n-C(=O)-O-(CH2) n -, where n is an integer of 2 to 12, m is an integer of 2 to 6, and R 8 represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms. In addition, the hydrogen atom of -CH2- in each of the above groups may be substituted with a methyl group. P3 represents a polymerizable group.

[0043] The polymerizable group is not particularly limited, but a polymerizable group capable of radical polymerization or cationic polymerization is preferred. The radical polymerizable group may be a known radical polymerizable group, and is preferably an acryloyl group or a methacryloyl group. It is known that the polymerization rate of an acryloyl group is generally fast, and from the viewpoint of improving productivity, an acryloyl group is preferred, but a methacryloyl group can also be used as a polymerizable group for the high birefringence liquid crystal. The cationic polymerizable group may be a known cationic polymerizable group, such as an alicyclic ether group, a cyclic acetal group, a cyclic lactone group, a cyclic thioether group, a spiro orthoester group, or a vinyloxy group. Among these, an alicyclic ether group or a vinyloxy group is preferred, and an epoxy group, an oxetanyl group, or a vinyloxy group is more preferred. Particularly preferred examples of the polymerizable group include the following.

[0044] [ka]

[0045] In this specification, the "alkyl group" may be any of linear, branched, and cyclic, and examples thereof include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, an n-pentyl group, an isopentyl group, a neopentyl group, a 1,1-dimethylpropyl group, an n-hexyl group, an isohexyl group, a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, and a cyclohexyl group.

[0046] The method for manufacturing the optically anisotropic layer 12 is not particularly limited, but a method using a composition containing a polymerizable liquid crystal compound (e.g., a rod-shaped liquid crystal compound with reverse wavelength dispersion having a polymerizable group) (hereinafter, also simply referred to as a "polymerizable liquid crystal composition") is preferred. The method using the polymerizable liquid crystal composition will be described in detail below.

[0047] The polymerizable liquid crystal composition contains the above-mentioned polymerizable liquid crystal compound. The polymerizable liquid crystal composition may contain other components in addition to the polymerizable liquid crystal compound. The other components include a polymerization initiator. The polymerization initiator used is selected according to the type of polymerization reaction, and examples of the polymerization initiator include a thermal polymerization initiator and a photopolymerization initiator. The content of the polymerization initiator in the polymerizable liquid crystal composition is preferably from 0.01 to 20% by mass, and more preferably from 0.5 to 10% by mass, based on the total solid content of the composition. The solid content means a component capable of forming an optically anisotropic layer from which the solvent has been removed, and even if the component is in a liquid state, it is considered to be a solid content.

[0048] The polymerizable liquid crystal compound may contain a polymerizable monomer other than the liquid crystal compound having a polymerizable group. The polymerizable monomer may be a radically polymerizable or cationic polymerizable compound, and a polyfunctional radically polymerizable monomer is preferable. The content of the polymerizable monomer in the polymerizable liquid crystal composition is preferably from 1 to 50% by mass, and more preferably from 2 to 30% by mass, based on the total mass of the liquid crystal compound.

[0049] Other components that may be contained in the polymerizable liquid crystal compound include, in addition to those mentioned above, a surfactant, an adhesion improver, a plasticizer, and a solvent. In order to make the polymerizable liquid crystal compound twisted, the polymerizable liquid crystal composition preferably contains a chiral agent. The chiral agent is added to twist the polymerizable liquid crystal compound, but of course, when the liquid crystal compound is a compound that shows optical activity, such as having an asymmetric carbon in the molecule, the addition of the chiral agent is not necessary. Also, depending on the manufacturing method and twist angle, the addition of the chiral agent is not necessary. The chiral agent is not particularly limited in structure as long as it is compatible with the polymerizable liquid crystal compound used in combination. Any known chiral agent (for example, described in "Liquid Crystal Device Handbook", Chapter 3, Section 4-3, Chiral Agents for TN and STN, p. 199, 1989, edited by the 142nd Committee of the Japan Society for the Promotion of Science) can be used. The amount of the chiral agent used is not particularly limited, and is adjusted so as to achieve the above-mentioned twist angle.

[0050] In order to tilt the liquid crystal compound, the polymerizable liquid crystal composition preferably contains an alignment control agent (vertical alignment agent, horizontal alignment agent). As the alignment control agent, a known compound can be used.

[0051] The optically anisotropic layer 12 can be produced by applying a polymerizable liquid crystal composition to form a coating film, performing an alignment treatment on the coating film to align the polymerizable liquid crystal compound, and then performing a hardening treatment. There is no particular limitation on the object to which the polymerizable liquid crystal composition is applied, and examples thereof include a support to be described later and a polarizer as described above. In order to orient the in-plane slow axis of the optically anisotropic layer to a predetermined direction, the substrate to which the polymerizable liquid crystal composition is applied may be subjected to a rubbing treatment. For example, a support that has been subjected to a rubbing treatment may be used.

[0052] Examples of the coating method of the polymerizable liquid crystal composition include curtain coating, dip coating, spin coating, print coating, spray coating, slot coating, roll coating, slide coating, blade coating, gravure coating, and wire bar coating.

[0053] Next, the formed coating film is subjected to an alignment treatment to align the polymerizable liquid crystal compound in the coating film. The alignment treatment can be carried out by drying the coating film at room temperature or by heating the coating film. In the case of a thermotropic liquid crystal compound, the liquid crystal phase formed by the alignment treatment can generally be transitioned by a change in temperature or pressure. In the case of a lyotropic liquid crystal compound, the transition can also be caused by a composition ratio such as the amount of solvent. The conditions for heating the coating are not particularly limited, but the heating temperature is preferably 50 to 250° C., more preferably 50 to 150° C., and the heating time is preferably 10 seconds to 10 minutes. After heating the coating film, the coating film may be cooled, if necessary, before the curing treatment (light irradiation treatment) described below. The cooling temperature is preferably 20 to 200°C, and more preferably 30 to 150°C.

[0054] Next, the coating film in which the polymerizable liquid crystal compound is aligned is subjected to a curing treatment. The method of hardening treatment performed on the coating film in which the polymerizable liquid crystal compound is oriented is not particularly limited, and examples thereof include light irradiation treatment and heat treatment. Among them, from the viewpoint of manufacturability, light irradiation treatment is preferred, and ultraviolet irradiation treatment is more preferred. The irradiation conditions for the light irradiation treatment are not particularly limited, but are preferably 50 to 1000 mJ / cm 2 is preferred. The atmosphere during the light irradiation treatment is not particularly limited, but a nitrogen atmosphere is preferred.

[0055] (other layers) The circularly polarizing plate 100A may have layers other than the polarizer 10 and the optically anisotropic layer 12 described above. The circularly polarizing plate 100A may have a support, which does not correspond to an optically anisotropic layer formed using a liquid crystal compound. The circularly polarizing plate 100 A may have a support between the polarizer 10 and the optically anisotropic layer 12 .

[0056] The support is preferably a transparent support, which means a support having a visible light transmittance of 60% or more, preferably 80% or more, and more preferably 90% or more.

[0057] The support may be a long support (long support). The length of the long support in the longitudinal direction is not particularly limited, but a support of 10 m or more is preferable, and from the viewpoint of productivity, a support of 100 m or more is preferable. The length in the longitudinal direction is not particularly limited, and is often 10,000 m or less. The width of the long support is not particularly limited, but is often 150 to 3000 mm, preferably 300 to 2000 mm.

[0058] The material for forming the support is preferably a polymer that is excellent in optical performance transparency, mechanical strength, thermal stability, moisture barrier properties, isotropy, and the like. Examples of polymer films that can be used as the support include cellulose acylate films (e.g., cellulose triacetate film, cellulose diacetate film, cellulose acetate butyrate film, and cellulose acetate propionate film), polyolefin films such as polyethylene and polypropylene, polyester films such as polyethylene terephthalate and polyethylene naphthalate, polyacrylic films such as polymethyl methacrylate, polyethersulfone films, polyurethane films, polycarbonate films, polysulfone films, polyether films, polymethylpentene films, polyether ketone films, (meth)acrylonitrile films, and films of polymers having an alicyclic structure (norbornene-based resins (Arton: product name, manufactured by JSR Corporation, amorphous polyolefins (Zeonex: product name, manufactured by Zeon Corporation))). Among these, triacetyl cellulose, polyethylene terephthalate, or a polymer having an alicyclic structure is preferable as the material for the polymer film.

[0059] The support may contain various additives (for example, an optical anisotropy adjusting agent, a wavelength dispersion adjusting agent, fine particles, a plasticizer, an ultraviolet protection agent, a deterioration inhibitor, and a release agent).

[0060] The retardation value (Rth(550)) in the thickness direction of the support at a wavelength of 550 nm is not particularly limited, but is preferably from −110 to 110 nm, and more preferably from −80 to 80 nm. The in-plane retardation value (Re(550)) of the support at a wavelength of 550 nm is not particularly limited, but is preferably from 0 to 50 nm, more preferably from 0 to 30 nm, and further preferably from 0 to 10 nm.

[0061] The thickness of the support is not particularly limited, but is preferably from 10 to 200 μm, more preferably from 10 to 100 μm, and even more preferably from 20 to 90 μm. The support may also be made up of a laminate of multiple sheets. The support may be subjected to a surface treatment (e.g., glow discharge treatment, corona discharge treatment, ultraviolet (UV) treatment, and flame treatment) on the surface thereof to improve adhesion with a layer applied thereon. In addition, an adhesive layer (undercoat layer) may be provided on the support. The support may be a so-called temporary support.

[0062] In addition, the surface of the support may be directly subjected to rubbing treatment. In other words, a support that has been subjected to rubbing treatment may be used. The direction of the rubbing treatment is not particularly limited, and an optimal direction is appropriately selected depending on the direction in which the liquid crystal compound is desired to be aligned. The rubbing treatment can be a treatment method that is widely used as a liquid crystal alignment treatment process for LCDs (liquid crystal displays), in which the surface of the support is rubbed in a certain direction with paper, gauze, felt, rubber, nylon fiber, polyester fiber, or the like to obtain alignment.

[0063] The circular polarizer 100A may have an alignment film. The alignment layer can be formed by such means as rubbing an organic compound (preferably a polymer), oblique deposition of an inorganic compound, formation of a layer with microgrooves, or deposition of an organic compound (e.g., ω-tricosanoic acid, dioctadecylmethylammonium chloride, methyl stearate) by the Langmuir-Blodgett technique (LB film). Furthermore, an alignment film is also known that exhibits an alignment function when an electric field is applied, a magnetic field is applied, or light (preferably polarized light) is irradiated. The alignment film is preferably formed by a rubbing treatment of a polymer.

[0064] The circularly polarizing plate 100A may have a pressure-sensitive adhesive layer, particularly on the surface of the optically anisotropic layer 12 opposite to the polarizer 10 side. As the adhesive constituting the adhesive layer, a known adhesive is used.

[0065] <Second embodiment> A second embodiment of the circular polarizer of the present invention will be described with reference to the drawings. Fig. 2 shows a schematic cross-sectional view of the second embodiment of the circular polarizer of the present invention. The circular polarizing plate 100B has a polarizer 10, a second optically anisotropic layer 16, and a first optically anisotropic layer 14 in this order. The first optically anisotropic layer 14 and the second optically anisotropic layer 16 are both layers formed using a rod-shaped liquid crystal compound LC. In particular, the first optically anisotropic layer 14 is a layer formed by fixing a liquid crystal compound with reverse wavelength dispersion that is twisted and aligned with the thickness direction as the helical axis, and the molecular axis of the rod-shaped liquid crystal compound LC in the first optically anisotropic layer is horizontal to the surface of the first optically anisotropic layer. That is, the rod-shaped liquid crystal compound LC shown in the first optically anisotropic layer 14 is twisted and aligned in the first optically anisotropic layer 14. In the circular polarizer 100B, the optically anisotropic layers formed using a liquid crystal compound include a first optically anisotropic layer 14 and a second optically anisotropic layer 16. That is, in the circular polarizer 100B, the optically anisotropic layer has a multilayer structure. Each layer will be described in detail below. Note that the polarizer 10 is the same as the polarizer 10 described in the first embodiment above, and therefore a description thereof will be omitted.

[0066] (First optically anisotropic layer 14) As shown in FIG. 2, the first optically anisotropic layer 14 is a layer in which a rod-shaped liquid crystal compound LC is fixed, which is twisted and aligned with the thickness direction (z-axis direction in FIG. 1) as the helical axis, and the molecular axis of the rod-shaped liquid crystal compound LC in the first optically anisotropic layer 14 is horizontal to the surface of the first optically anisotropic layer 14. The first optically anisotropic layer 14 is preferably a layer in which a chiral nematic phase having a so-called helical structure is fixed. In other words, the first optically anisotropic layer 14 is preferably a layer in which a liquid crystal compound is twisted and aligned with the thickness direction as the helical axis, and whose molecular axis is aligned horizontally is fixed. In addition, when forming the above phase, it is preferable to use a mixture of a liquid crystal compound exhibiting a nematic liquid crystal phase and a chiral agent described later. The meaning of the "fixed" state is as described above. The molecular axis being parallel to the surface of the optically anisotropic layer is defined as described in the first embodiment above.

[0067] The twist angle of the rod-shaped liquid crystal compound LC (the twist angle of the alignment direction of the rod-shaped liquid crystal compound LC) is preferably within a range of 85±20°. That is, the twist angle is preferably 65 to 105°. Among them, in terms of better effects of the present invention, 75 to 95° is more preferable, and 80 to 90° is even more preferable. The liquid crystal compound being twisted means that the liquid crystal compound is twisted from one main surface to the other main surface of the first optically anisotropic layer 14 around the axis in the thickness direction of the first optically anisotropic layer 14. Accordingly, the orientation direction (in-plane slow axis direction) of the liquid crystal compound differs depending on the position in the thickness direction of the first optically anisotropic layer 14. In addition, there are two kinds of twist directions, which may be right-handed or left-handed. In Fig. 2, right-handed twist means that when observed from the polarizer 10 toward the first optically anisotropic layer 14, the in-plane slow axis of the first optically anisotropic layer 14 on the opposite side to the polarizer 10 side is positioned clockwise with respect to the in-plane slow axis of the first optically anisotropic layer 14 on the polarizer 10 side, which serves as the reference axis.

[0068] The torsion angle is measured using an AxoScan (polarimeter) device manufactured by Axometrics Inc. and the device analysis software of the same company.

[0069] It is preferable that the value of the product Δn1d1 of the refractive index anisotropy Δn1 of the first optically anisotropic layer 14 measured at a wavelength of 550 nm and the thickness d1 of the first optically anisotropic layer 14 satisfy the relationship of formula (1) in terms of superior effects of the present invention. Formula (1) 150nm≦Δn1d1≦230nm Among these, it is more preferable that the relationship of formula (1A) is satisfied, and it is even more preferable that the relationship of formula (1B) is satisfied. Formula (1A) 160nm≦Δn1d1≦220nm Formula (1B) 170nm≦Δn1d1≦210nm The above Δn1d1 is measured using an AxoScan (polarimeter) device manufactured by Axometrics Inc. and the device analysis software of the same company, in the same manner as in the measurement of the torsion angle.

[0070] (Second optically anisotropic layer 16) The second optically anisotropic layer 16 is a layer formed using a rod-shaped liquid crystal compound LC. More specifically, the second optically anisotropic layer 16 is a layer formed using a composition containing the rod-shaped liquid crystal compound LC. The second optically anisotropic layer 16 is different from the first optically anisotropic layer 14 and is a layer in which homogeneously aligned liquid crystal compounds are fixed. The meaning of the "fixed" state is as described above.

[0071] In this specification, homogeneous orientation refers to a state in which the molecular axis of a liquid crystal compound (for example, the long axis in the case of a rod-shaped liquid crystal compound) is aligned horizontally and in the same direction relative to the layer surface (optical uniaxiality). Here, "horizontal" does not necessarily mean strictly horizontal, but means that the average molecular axis of the liquid crystal compound in the layer forms an inclination angle of less than 20° with the layer surface. In addition, the same orientation does not require the orientation to be strictly the same, but rather means that when the orientations of the slow axes are measured at any 20 positions within the plane, the maximum difference between the slow axis orientations at the 20 positions (the difference between the two slow axis orientations with the largest difference among the 20 slow axis orientations) is less than 10°.

[0072] It is preferable that the value of the product Δn2d2 of the refractive index anisotropy Δn2 of the second optically anisotropic layer 16 measured at a wavelength of 550 nm and the thickness d2 of the second optically anisotropic layer 16 satisfy the relationship of formula (2) in terms of superior effects of the present invention. Formula (2) 140nm≦Δn2d2≦220nm Among these, it is more preferable that the relationship of formula (2A) is satisfied, and it is even more preferable that the relationship of formula (2B) is satisfied. Formula (2A) 180nm≦Δn2d2≦220nm Formula (2B) 190nm≦Δn2d2≦210nm The above Δn2d2 is measured using an AxoScan (polarimeter) device manufactured by Axometrics, Inc., using the device analysis software of the same company.

[0073] The in-plane slow axis of the first optically anisotropic layer 14 on the surface facing the second optically anisotropic layer 16 is parallel to the in-plane slow axis of the second optically anisotropic layer 16 on the surface facing the first optically anisotropic layer 14. The definition of parallel is as described above. That is, the angle formed by the in-plane slow axis of the first optically anisotropic layer 14 on the surface facing the second optically anisotropic layer 16 and the in-plane slow axis of the second optically anisotropic layer 16 on the surface facing the first optically anisotropic layer 14 is within 10° (0 to 10°).

[0074] An alignment film, which will be described later, may be disposed between the first optically anisotropic layer 14 and the second optically anisotropic layer 16, but as shown in Fig. 2, it is preferable that the first optically anisotropic layer 14 and the second optically anisotropic layer 16 are adjacent to each other and there is substantially no alignment film between the first optically anisotropic layer 14 and the second optically anisotropic layer 16. When there is substantially no alignment film between the first optically anisotropic layer 14 and the second optically anisotropic layer 16, the covalent bonds between the compounds contained in each optically anisotropic layer can be utilized, resulting in more excellent adhesion. As described above, since the first optically anisotropic layer 14 contains a twisted liquid crystal compound, a circular polarizer can be obtained without performing a rubbing treatment. More specifically, when the second optically anisotropic layer 16 is formed on the first optically anisotropic layer 14 using a liquid crystal compound after the first optically anisotropic layer 14 is produced, the direction of the in-plane slow axis is different between the surface 141 on the second optically anisotropic layer 16 side of the first optically anisotropic layer 14 and the surface 142 on the opposite side to the second optically anisotropic layer 16 side, and if the liquid crystal compound is applied on the surface 141 without performing a rubbing treatment, the liquid crystal compound will be aligned along the alignment state of the surface 141, and a desired optically anisotropic layer can be obtained.

[0075] In FIG. 2, the first optically anisotropic layer 14 and the second optically anisotropic layer 16 are formed using rod-like liquid crystal compounds, but the present invention is not limited to this embodiment. The embodiment of the liquid crystal compound having reverse wavelength dispersion used in forming the first optically anisotropic layer 14 and the second optically anisotropic layer 16 is as explained in the first embodiment above.

[0076] In the circular polarizing plate 100B, the relationship between the absorption axis of the polarizer 10 and the in-plane slow axes of the first optically anisotropic layer 14 and the second optically anisotropic layer 16 preferably satisfies the following requirement (Xa) or (Ya). (Xa) The angle between the in-plane slow axis of the second optically anisotropic layer 16 and the absorption axis of the polarizer 10 is within the range of 13±10° (3 to 23°) (preferably within the range of 13±6°, more preferably within the range of 13±3°). (Ya) The angle between the in-plane slow axis of the second optically anisotropic layer 16 and the absorption axis of the polarizer 10 is within the range of 103±10° (93 to 113°) (preferably within the range of 103±6°, and more preferably within the range of 103±3°). As described above, the in-plane slow axis of the surface of the first optically anisotropic layer 14 facing the second optically anisotropic layer 16 is parallel to the in-plane slow axis of the surface of the second optically anisotropic layer 16 facing the first optically anisotropic layer 14.

[0077] The relationship between the absorption axis of the polarizer 10, the in-plane slow axis of the second optically anisotropic layer 16, and the in-plane slow axis of the first optically anisotropic layer 14 in the requirement represented by (Xa) above will be described in more detail with reference to FIG. 3. The arrow in the polarizer 10 in Fig. 3 indicates the absorption axis, and the arrows in the second optically anisotropic layer 16 and the first optically anisotropic layer 14 indicate the in-plane slow axis in each layer. Fig. 4 also shows the relationship between the absorption axis of the polarizer 10, the in-plane slow axis of the second optically anisotropic layer 16, and the in-plane slow axis of the first optically anisotropic layer 14 when observed from the white arrow in Fig. 3. In FIG. 4, the rotation angle of the in-plane slow axis is expressed as a positive value in the counterclockwise direction and a negative value in the clockwise direction with respect to the absorption axis of the polarizer 10 when observed from the white arrow in FIG.

[0078] In Fig. 3, the angle φ1a between the absorption axis of the polarizer 10 and the in-plane slow axis of the second optically anisotropic layer 16 is 13°. That is, the in-plane slow axis of the second optically anisotropic layer 16 is rotated by -13° (13° clockwise) with respect to the absorption axis of the polarizer 10. Note that Fig. 3 shows an embodiment in which the in-plane slow axis of the second optically anisotropic layer 16 is at a position of -13°, but is not limited to this embodiment and may be in the range of -13±10°. As described above, the second optically anisotropic layer 16 has the same in-plane slow axis at both interfaces. That is, the angle φ2a between the absorption axis of the polarizer 10 and the in-plane slow axis at the surface 162 on the first optically anisotropic layer 14 side is approximately the same as the angle φ1a.

[0079] 3, the in-plane slow axis of the second optically anisotropic layer 16 at the surface 162 facing the first optically anisotropic layer 14 is parallel to the in-plane slow axis of the first optically anisotropic layer 14 at the surface 141 facing the second optically anisotropic layer 16. In other words, the angle φ3a between the absorption axis of the polarizer 10 and the in-plane slow axis of the first optically anisotropic layer 14 at the surface 141 facing the second optically anisotropic layer 16 is approximately the same as the above-mentioned φ1a.

[0080] The in-plane slow axis of the first optically anisotropic layer 14 at the surface 141 facing the second optically anisotropic layer 16 and the in-plane slow axis of the first optically anisotropic layer 14 at the surface 142 opposite to the second optically anisotropic layer 16 form the twist angle described above. Here, taking the twist angle of 85° as an example as shown in Fig. 3, the in-plane slow axis of the optically anisotropic layer 12 rotates by -85° (85° clockwise). Therefore, the angle φ4a between the absorption axis of the polarizer 10 and the in-plane slow axis of the first optically anisotropic layer 14 at the surface 142 is 98°. In addition, in FIG. 3, the in-plane slow axis at surface 142 of the first optically anisotropic layer 14 is shown rotated 85° clockwise relative to the in-plane slow axis at surface 141 of the first optically anisotropic layer 14, but this is not limited to this embodiment, and the rotation angle may be in the range of 65 to 105° clockwise.

[0081] 3, the in-plane slow axis of the second optically anisotropic layer 16 is at a position of 13° clockwise with respect to the absorption axis of the polarizer 10, and the twist direction of the liquid crystal compound in the first optically anisotropic layer 14 is clockwise (right-handed twist). The twist direction is observed from the white arrow in Fig. 3, and is judged to be right-handed or left-handed with reference to the in-plane slow axis on the surface (surface 141) of the first optically anisotropic layer 14 facing the polarizer 10. 3, the in-plane slow axis of the second optically anisotropic layer 16 and the twist direction of the liquid crystal compound in the first optically anisotropic layer 14 are clockwise in detail, but they may be counterclockwise as long as a predetermined angular relationship is satisfied. More specifically, the in-plane slow axis of the second optically anisotropic layer 16 may be at a position of 13° counterclockwise with respect to the absorption axis of the polarizer 10, and the twist direction of the liquid crystal compound in the first optically anisotropic layer 14 may be counterclockwise (left twist). To summarize these aspects, when the second optically anisotropic layer 16 is observed from the polarizer 10 and counterclockwise is represented by a positive angle value, the absorption axis of the polarizer 10 is taken as the reference (0°) and the in-plane slow axis of the second optically anisotropic layer 16 is in the range of 13±10° and the twist direction of the first optically anisotropic layer 14 is counterclockwise, or the in-plane slow axis of the second optically anisotropic layer 16 is in the range of -13±10° and the twist direction of the first optically anisotropic layer 14 is clockwise.

[0082] Next, the relationship between the absorption axis of the polarizer 10 in the embodiment represented by (Ya) above, the in-plane slow axis of the second optically anisotropic layer 16, and the in-plane slow axis of the first optically anisotropic layer 14 will be described in more detail with reference to FIG. 5. The arrow in the polarizer 10 in Fig. 5 represents the absorption axis, and the arrows in the second optically anisotropic layer 16 and the first optically anisotropic layer 14 represent the in-plane slow axis in each layer. Fig. 6 shows the relationship between the absorption axis of the polarizer 10, the in-plane slow axis of the second optically anisotropic layer 16, and the in-plane slow axis of the first optically anisotropic layer 14 when observed from the white arrow in Fig. 5. 6, the rotation angle of the in-plane slow axis is expressed as a positive value in the counterclockwise direction and a negative value in the clockwise direction with respect to the absorption axis of the polarizer 10 when observed from the white arrow in FIG.

[0083] The embodiment shown in FIG. 5 has the same configuration as the embodiment shown in FIG. 3, except that the absorption axis of the polarizer 10 differs by 90° from the absorption axis of the polarizer 10 in FIG. In Fig. 5, the angle φ1a between the absorption axis of the polarizer 10 and the in-plane slow axis of the second optically anisotropic layer 16 is 103°. That is, the in-plane slow axis of the second optically anisotropic layer 16 is rotated by -103° (103° clockwise) with respect to the absorption axis of the polarizer 10. Note that Fig. 5 shows an embodiment in which the in-plane slow axis of the second optically anisotropic layer 16 is at a position of -103°, but is not limited to this embodiment and may be in the range of -103±10°. As described above, the second optically anisotropic layer 16 has the same in-plane slow axis at both interfaces. That is, the angle φ2a between the absorption axis of the polarizer 10 and the in-plane slow axis at the surface 162 on the optically anisotropic layer 12 side is approximately the same as the above angle φ1a.

[0084] 5, similarly to Fig. 3, the in-plane slow axis of the second optically anisotropic layer 16 at the surface 162 facing the first optically anisotropic layer 14 is parallel to the in-plane slow axis of the first optically anisotropic layer 14 at the surface 141 facing the second optically anisotropic layer 16. In other words, the angle φ3a between the absorption axis of the polarizer 10 and the in-plane slow axis of the first optically anisotropic layer 14 at the surface 141 facing the second optically anisotropic layer 16 is approximately the same as the above-mentioned φ1a.

[0085] In Fig. 5, similarly to Fig. 3, the in-plane slow axis at the surface 141 of the first optically anisotropic layer 14 facing the second optically anisotropic layer 16 and the in-plane slow axis at the surface 142 of the first optically anisotropic layer 14 facing away from the second optically anisotropic layer 16 form the twist angle described above. Here, taking the twist angle of 85° as shown in Fig. 3 as an example, the in-plane slow axis of the optically anisotropic layer 12 rotates by -85° (85° clockwise). Therefore, the angle φ4a between the absorption axis of the polarizer 10 and the in-plane slow axis at the surface 142 of the first optically anisotropic layer 14 is 188°.

[0086] 5, the in-plane slow axis of the second optically anisotropic layer 16 is at -103° with respect to the absorption axis of the polarizer 10, and the twist direction of the liquid crystal compound in the first optically anisotropic layer 14 is clockwise (right-handed twist). The twist direction is observed from the white arrow in Fig. 5, and is judged to be right-handed or left-handed with reference to the in-plane slow axis on the surface (surface 141) of the first optically anisotropic layer 14 facing the polarizer 10. 5, the in-plane slow axis of the second optically anisotropic layer 16 and the twist direction of the liquid crystal compound in the first optically anisotropic layer 14 are clockwise in detail, but they may be counterclockwise as long as a predetermined angular relationship is satisfied. More specifically, the in-plane slow axis of the second optically anisotropic layer 16 may be at a position of 103° with respect to the absorption axis of the polarizer 10, and the twist direction of the liquid crystal compound in the first optically anisotropic layer 14 may be counterclockwise (left twist). To summarize these aspects, when the second optically anisotropic layer 16 is observed from the polarizer 10 and counterclockwise is represented by a positive angle value, the absorption axis of the polarizer 10 is taken as the reference (0°), and the in-plane slow axis of the second optically anisotropic layer 16 is in the range of 103±10° and the twist direction of the first optically anisotropic layer 14 is counterclockwise, or the in-plane slow axis of the second optically anisotropic layer 16 is in the range of -103±10° and the twist direction of the first optically anisotropic layer 14 is clockwise. Of the embodiment shown in FIG. 3 (requirement (Xa)) and the embodiment shown in FIG. 5 (requirement (Ya)), the embodiment shown in FIG. 3 is more preferable.

[0087] (other layers) The circularly polarizing plate 100B may have layers other than the polarizer 10, the second optically anisotropic layer 16, and the first optically anisotropic layer . The circular polarizing plate 100B may have a support. The form of the support is as described in the first embodiment. The circular polarizing plate 100B may have a support between the polarizer 10 and the second optically anisotropic layer 16. The circularly polarizing plate 100B may have an alignment film. The aspect of the alignment film is as explained in the first embodiment. The circularly polarizing plate 100B may have a pressure-sensitive adhesive layer. In particular, the pressure-sensitive adhesive layer may be provided on the surface of the first optically anisotropic layer 14 opposite to the polarizer 10. As the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer, a known pressure-sensitive adhesive is used.

[0088] (Manufacturing method) The method for producing the circularly polarizing plate is not particularly limited, and may be a known method. The circularly polarizing plate may be produced continuously by roll-to-roll production. For example, a circular polarizing plate can be manufactured by preparing a first optically anisotropic layer and a second optically anisotropic layer each exhibiting a predetermined optical property, and bonding the optically anisotropic layer and the polarizer together in a predetermined order via an adhesive layer (e.g., a pressure-sensitive adhesive layer or an adhesive layer). Alternatively, a first optically anisotropic layer and a second optically anisotropic layer may be sequentially formed on a support using a polymerizable liquid crystal composition to produce an optical film, and the optical film obtained may be laminated to a polarizer to produce a circularly polarizing plate. For example, a polymerizable liquid crystal composition may be applied onto a support to form a second optically anisotropic layer, and then a polymerizable liquid crystal composition may be applied onto the second optically anisotropic layer to form a first optically anisotropic layer. The form of the polymerizable liquid crystal composition and the procedure of the method for producing an optically anisotropic layer using the polymerizable liquid crystal composition are as described in the first embodiment.

[0089] When producing the first optically anisotropic layer and the second optically anisotropic layer, the following steps 1 to 5 may be carried out. By carrying out the following steps 1 to 5, a laminate of the first optically anisotropic layer and the second optically anisotropic layer can be produced in a single coating step. Step 1: A step of applying a polymerizable liquid crystal composition containing a chiral agent including at least a photosensitive chiral agent whose helical twisting power changes upon irradiation with light, and a liquid crystal compound having a reverse wavelength dispersion property and a polymerizable group (hereinafter, in the explanation of steps 1 to 5, this is also simply referred to as a "liquid crystal compound") onto a support to form a composition layer. Step 2: A step of subjecting the composition layer to a heat treatment to align the liquid crystal compound in the composition layer. Step 3: After step 2, a step of irradiating the composition layer with light under conditions of an oxygen concentration of 1% by volume or more. Step 4: After step 3, a step of subjecting the composition layer to a heat treatment. Step 5: After step 4, the composition layer is subjected to a curing treatment to fix the alignment state of the liquid crystal compound and form a first optically anisotropic layer and a second optically anisotropic layer. The procedures for each of the above steps will be described in detail below.

[0090] [Process 1] Step 1 is a step of forming a composition layer by applying a polymerizable liquid crystal composition containing at least a chiral agent including a photosensitive chiral agent whose helical twisting power changes upon irradiation with light, a liquid crystal compound having a reverse wavelength dispersion and a polymerizable group, and an alignment control agent onto a support. By carrying out this step, a composition layer to be subjected to a light irradiation treatment described later is formed. The various components contained in the polymerizable liquid crystal composition are as described above, and the photosensitive chiral agent not described above will be described in detail below. The helical twisting power (HTP) of a chiral agent is a factor indicating the helical orientation ability represented by the following formula (X). Formula (X) HTP = 1 / (helix pitch length (unit: μm) × concentration of chiral agent relative to liquid crystal compound (mass%)) [μm -1 ] The helical pitch length refers to the length of the pitch P (=helical period) of the helical structure of a cholesteric liquid crystal phase, and can be measured by the method described on page 196 of Liquid Crystal Handbook (published by Maruzen Co., Ltd.).

[0091] The photosensitive chiral agent (hereinafter, simply referred to as "chiral agent A") whose helical twisting power changes upon irradiation with light may be liquid crystalline or non-liquid crystalline. Generally, chiral agent A often contains an asymmetric carbon atom. Note that chiral agent A may be an axially asymmetric compound or a planar asymmetric compound that does not contain an asymmetric carbon atom. The chiral agent A may have a polymerizable group.

[0092] The chiral agent A may be a chiral agent whose helical twisting power increases or decreases upon irradiation with light, and is preferably a chiral agent whose helical twisting power decreases upon irradiation with light. In this specification, "increase and decrease in helical twisting power" refers to an increase or decrease when the initial helical direction (before light irradiation) of the chiral agent A is taken as "positive." Therefore, even when the helical twisting power continues to decrease upon light irradiation and exceeds 0, causing the helical direction to become "negative" (i.e., when a helical direction opposite to the initial helical direction (before light irradiation) is induced), this also corresponds to "a chiral agent whose helical twisting power decreases."

[0093] An example of the chiral agent A is a so-called photoreactive chiral agent. The photoreactive chiral agent has a chiral moiety and a photoreactive moiety that undergoes a structural change upon irradiation with light, and is a compound that, for example, significantly changes the twisting power of a liquid crystal compound depending on the amount of irradiation. Among them, the chiral agent A is preferably a compound having at least a photoisomerization site, and more preferably the photoisomerization site has a photoisomerizable double bond. As the photoisomerization site having the photoisomerizable double bond, a cinnamoyl site, a chalcone site, an azobenzene site, or a stilbene site is preferable because photoisomerization is easily caused and the difference in helical induction power before and after light irradiation is large, and a cinnamoyl site, a chalcone site, or a stilbene site is more preferable because the absorption of visible light is small. The photoisomerization site corresponds to the photoreactive site whose structure changes by light irradiation described above.

[0094] At least the above-mentioned chiral agent A is used in step 1. Step 1 may be an embodiment in which two or more types of chiral agents A are used, or may be an embodiment in which at least one type of chiral agent A and at least one type of chiral agent whose helical twisting power does not change upon irradiation with light (hereinafter, also simply referred to as "chiral agent B") are used. The chiral agent B may be liquid crystalline or non-liquid crystalline. The chiral agent B generally contains an asymmetric carbon atom. The chiral agent B may be an axially asymmetric compound or a planar asymmetric compound that does not contain an asymmetric carbon atom. The chiral agent B may have a polymerizable group. As the chiral agent B, a known chiral agent can be used. Chiral agent B is preferably a chiral agent that induces a helical twist in the opposite direction to that of the above-mentioned chiral agent A. That is, for example, when the helical twist induced by chiral agent A is right-handed, the helical twist induced by chiral agent B is left-handed.

[0095] The content of the chiral agent A in the composition layer is not particularly limited, but in order to facilitate uniform alignment of the liquid crystal compound, it is preferably 5.0% by mass or less, more preferably 3.0% by mass or less, even more preferably 2.0% by mass or less, particularly preferably less than 1.0% by mass, more particularly preferably 0.8% by mass or less, and most preferably 0.5% by mass or less, relative to the total mass of the liquid crystal compound. The lower limit is not particularly limited, but is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and even more preferably 0.05% by mass or more. The chiral agent A may be used alone or in combination of two or more. When two or more chiral agents A are used in combination, the total content is preferably within the above range.

[0096] The content of the chiral agent B in the composition layer is not particularly limited, but in terms of facilitating uniform alignment of the liquid crystal compound, it is preferably 5.0% by mass or less, more preferably 3.0% by mass or less, even more preferably 2.0% by mass or less, particularly preferably less than 1.0% by mass, more particularly preferably 0.8% by mass or less, and most preferably 0.5% by mass or less, relative to the total mass of the liquid crystal compound. The lower limit is not particularly limited, but it is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and even more preferably 0.05% by mass or more. The chiral agent B may be used alone or in combination of two or more. When two or more chiral agents B are used in combination, the total content is preferably within the above range.

[0097] The total content of the chiral dopant in the composition layer (total content of all chiral dopant) is preferably 5.0% by mass or less, more preferably 4.0% by mass or less, even more preferably 2.0% by mass or less, and particularly preferably 1.0% by mass or less, based on the total mass of the liquid crystal compound. There is no particular lower limit, but it is preferably 0.01% by mass or more, more preferably 0.02% by mass or more, and even more preferably 0.05% by mass or more.

[0098] The method for forming a composition layer by applying the polymerizable liquid crystal composition is not particularly limited, and examples thereof include the above-mentioned methods for applying the polymerizable liquid crystal composition.

[0099] The thickness of the composition layer is not particularly limited, but is preferably from 0.1 to 20 μm, more preferably from 0.2 to 15 μm, and even more preferably from 0.5 to 10 μm.

[0100] [Process 2] Step 2 is a step of aligning the liquid crystal compound in the composition layer by subjecting the composition layer to a heat treatment. By carrying out this step, the liquid crystal compound in the composition layer is brought into a predetermined alignment state. The optimum conditions for the heat treatment are selected depending on the liquid crystal compound used. Among these, the heating temperature is often 10 to 250°C, more often 40 to 150°C, and even more often 50 to 130°C. The heating time is often 0.1 to 60 minutes, and more often 0.2 to 5 minutes.

[0101] The absolute value of the weighted average helical twisting power of the chiral agent in the composition layer formed in step 1 is 0.0 to 1.9 μm -1 It is preferable that the thickness is 0.0 to 1.5 μm. -1 More preferably, the thickness is 0.0 to 1.0 μm. -1 More preferably, the thickness is 0.0 to 0.5 μm. -1 is particularly preferred, with zero being most preferred.

[0102] The weighted average helical twisting power of the chiral agent means, when two or more kinds of chiral agents are contained in the composition layer, the sum of the product of the helical twisting power of each chiral agent contained in the composition layer and the concentration (mass%) of each chiral agent in the composition layer divided by the total concentration (mass%) of the chiral agents in the composition layer. For example, when two kinds of chiral agents (chiral agent X and chiral agent Y) are used in combination, it is represented by the following formula (Y). Equation (Y) Weighted average helical induced force (μm -1 )=(helix-inducing power of chiral agent X (μm -1 ) × concentration of chiral dopant X in the composition layer (% by mass) + helical twisting power of chiral dopant Y (μm -1 ) × concentration of chiral agent Y in the composition layer (mass%) / (concentration of chiral agent X in the composition layer (mass%) + concentration of chiral agent Y in the composition layer (mass%)) However, in the above formula (Y), when the helical direction of the chiral agent is right-handed, the helical twisting power is a positive value. On the other hand, when the helical direction of the chiral agent is left-handed, the helical twisting power is a negative value. That is, for example, when the helical twisting power is 10 μm -1 In the case of the chiral agent, when the helical direction of the helix induced by the chiral agent is right-handed, the helical induction force is 10 μm-1 On the other hand, when the helical direction of the helix induced by the chiral agent is left-handed, the helical induction force is expressed as -10 μm -1 It is expressed as:

[0103] When the absolute value of the weighted average helical twisting power of the chiral agent in the composition layer formed by step 1 is 0, a composition layer 20 in which rod-shaped liquid crystal compounds LC with reverse wavelength dispersion are aligned is formed on a support 18, as shown in Figure 7. 7 is a schematic diagram of a cross section of a support 18 and a composition layer 20. In the composition layer 20 shown in FIG. 7, chiral agents A and B are present at the same concentration, and the helical direction induced by chiral agent A is left-handed, and the helical direction induced by chiral agent B is right-handed. In addition, the absolute value of the helical twisting power of chiral agent A and the absolute value of the helical twisting power of chiral agent B are the same.

[0104] [Process 3] Step 3 is a step of irradiating the composition layer with light in the presence of oxygen after step 2. The mechanism of this step will be described below with reference to the drawings. As shown in Fig. 8, in the above-mentioned step 2, light irradiation is performed from the direction opposite to the composition layer 20 side of the support 18 (the direction of the white arrow in Fig. 8) under conditions of an oxygen concentration of 1% by volume or more. Note that, although light irradiation is performed from the support 18 side in Fig. 8, it may be performed from the composition layer 20 side. In this case, when comparing the first region 20A on the support 18 side of the composition layer 20 with the second region 20B on the opposite side to the support 18 side, the surface of the second region 20B is closer to the air, so the oxygen concentration in the second region 20B is higher and the oxygen concentration in the first region 20A is lower. Therefore, when the composition layer 20 is irradiated with light, polymerization of the liquid crystal compound is likely to proceed in the first region 20A, and the alignment state of the liquid crystal compound is fixed. Note that the chiral agent A is also present in the first region 20A, and the chiral agent A is also photosensitive, and the helical induction force changes. However, since the alignment state of the liquid crystal compound is fixed in the first region 20A, even if step 4, which will be described later, is performed to perform a heat treatment on the irradiated composition layer, the alignment state of the liquid crystal compound does not change. In addition, since the oxygen concentration is high in the second region 20B, even if light is irradiated, the polymerization of the liquid crystal compound is inhibited by oxygen, and the polymerization does not proceed easily. Since the chiral agent A is also present in the second region 20B, the chiral agent A is exposed to light and the helical twisting power changes. Therefore, when step 4 (heat treatment) described later is performed, the alignment state of the liquid crystal compound changes according to the changed helical twisting power.

[0105] That is, by carrying out step 3, fixation of the alignment state of the liquid crystal compound is facilitated in the region of the composition layer on the substrate side, whereas fixation of the alignment state of the liquid crystal compound is difficult in the region of the composition layer on the opposite side to the substrate side, resulting in a state in which the helical twisting power changes depending on the photoexposed chiral dopant A.

[0106] Step 3 is carried out under conditions of an oxygen concentration of 1% by volume or more. In particular, the oxygen concentration is preferably 2% by volume or more, more preferably 5% by volume or more, in that regions in which the alignment state of the liquid crystal compound is different are easily formed in the optically anisotropic layer. The upper limit is not particularly limited, but may be 100% by volume.

[0107] The irradiation intensity of the light irradiation in step 3 is not particularly limited and can be appropriately determined based on the helical twisting power of the chiral agent A. The irradiation amount of the light irradiation in step 3 is not particularly limited, but it is preferably 300 mJ / cm from the viewpoint of facilitating the formation of a desired optically anisotropic layer. 2 Less than 200 mJ / cm is preferable. 2 The lower limit is 5 mJ / cm2, which is more preferable because it is easy to form a desired optically anisotropic layer. 2 More than 10 mJ / cm is preferable. 2 The above is more preferable. The light irradiation in step 3 is preferably carried out at a temperature of 15 to 70°C (preferably 15 to 50°C).

[0108] The light used for the photoirradiation may be any light to which the chiral agent A is photosensitive. In other words, the light used for the photoirradiation is not particularly limited as long as it is an actinic ray or radiation that changes the helical twisting power of the chiral agent A, and examples of the light include the bright line spectrum of a mercury lamp, far ultraviolet light represented by an excimer laser, extreme ultraviolet light, X-rays, ultraviolet light, and electron beams. Among these, ultraviolet light is preferred.

[0109] [Step 4] Step 4 is a step of subjecting the composition layer to a heat treatment after step 3. By carrying out this step, the alignment state of the liquid crystal compound is changed in a region in the composition layer irradiated with light where the helical twisting power of the chiral dopant A has been changed. The mechanism of this process will be explained below with reference to the drawings.

[0110] As described above, when step 3 is performed on the composition layer 20 shown in FIG. 8, the orientation state of the liquid crystal compound is fixed in the first region 20A, whereas the polymerization of the liquid crystal compound is difficult to proceed in the second region 20B, and the orientation state of the liquid crystal compound is not fixed. Moreover, the helical twisting power of the chiral agent A changes in the second region 20B. When such a change in the helical twisting power of the chiral agent A occurs, the force twisting the liquid crystal compound changes in the second region 20B compared to the state before light irradiation. This point will be explained in more detail. As described above, chiral agent A and chiral agent B are present in the composition layer 20 shown in Fig. 8 at the same concentration, the helical direction induced by chiral agent A is left-handed, and the helical direction induced by chiral agent B is right-handed. Furthermore, the absolute value of the helical twisting power of chiral agent A is the same as that of chiral agent B. Therefore, the weighted average helical twisting power of the chiral agents in the composition layer before light irradiation is 0. The above embodiment is shown in Figure 9. In Figure 9, the vertical axis indicates the helical twisting power of the chiral agent (μm -1 The horizontal axis represents the "light irradiation dose (mJ / cm ) × the concentration of the chiral agent (mass%)", and the further away from zero the value is, the stronger the helical twisting power is. 2 )". First, the relationship between chiral agent A and chiral agent B in the composition layer before light irradiation corresponds to the time when the amount of light irradiation is 0, and the "helix induction power of chiral agent A (μm -1 ) × concentration of chiral agent A (mass%) and the helical twisting power of chiral agent B (μm -1 This corresponds to a state in which the absolute value of "the helical twist induction potential (mass%) × the concentration (mass%) of chiral dopant B" is equal to that of chiral dopant A. In other words, the helical twist induction potential of chiral dopant A, which induces left-handedness, and that of chiral dopant B, which induces right-handedness, are offset. When light is irradiated to second region 20B in this state, and the helical twisting power of chiral agent A decreases depending on the amount of light irradiation as shown in Fig. 9, the weighted average helical twisting power of the chiral agent in second region 20B increases, and the right-handed helical twisting power becomes stronger, as shown in Fig. 10. In other words, the helical twisting power of the liquid crystal compound increases in the direction (+) of the helical twist induced by chiral agent B as the amount of irradiation increases. Therefore, when the composition layer 20 after step 3, in which such a change in the weighted average helical twisting force has occurred, is subjected to a heat treatment to promote reorientation of the liquid crystal compound, as shown in Figure 11, in the second region 20B, the liquid crystal compound LC is twisted and aligned along the helical axis extending along the thickness direction of the composition layer 20. On the other hand, as described above, in the first region 20A of the composition layer 20, the polymerization of the liquid crystal compound has progressed during step 3, and the orientation state of the liquid crystal compound has been fixed, so that reorientation of the liquid crystal compound does not proceed. As described above, by carrying out step 4, a plurality of regions in which the liquid crystal compound has a different alignment state are formed along the thickness direction of the composition layer. The degree of twist of the liquid crystal compound LC can be appropriately adjusted by the type of chiral dopant A used, the exposure dose in step 3, and the like, to realize a desired twist angle.

[0111] In the above, the embodiment in which a chiral agent whose helical twisting power decreases upon irradiation with light is used as the chiral agent A has been described, but the present invention is not limited to this embodiment. For example, a chiral agent whose helical twisting power increases upon irradiation with light may be used as the chiral agent A. In this case, the helical twisting power induced by the chiral agent A increases upon irradiation with light, and the liquid crystal compound is twisted in the direction of rotation induced by the chiral agent A. In addition, in the above, the embodiment in which the chiral agent A and the chiral agent B are used in combination has been described, but the present invention is not limited to this embodiment. For example, the present invention may be an embodiment in which two types of chiral agents A are used. Specifically, the present invention may be an embodiment in which the chiral agent A1 that induces left-handedness and the chiral agent A2 that induces right-handedness are used in combination. The chiral agents A1 and A2 may each independently be a chiral agent that increases the helical induction power, or a chiral agent that decreases the helical induction power. For example, a chiral agent that induces left-handedness and whose helical induction power increases upon light irradiation and a chiral agent that induces right-handedness and whose helical induction power decreases upon light irradiation may be used in combination.

[0112] The optimum conditions for the heat treatment are selected depending on the liquid crystal compound used. Among these, the heating temperature is preferably the temperature to which the material is heated from the state in step 3, which is often 35 to 250°C, more often 50 to 150°C, even more often higher than 50°C and up to 150°C, and particularly often 60 to 130°C. The heating time is often 0.01 to 60 minutes, and more often 0.03 to 5 minutes.

[0113] The absolute value of the weighted average helical twisting power of the chiral agent in the composition layer after light irradiation is not particularly limited, but the absolute value of the difference between the weighted average helical twisting power of the chiral agent in the composition layer after light irradiation and the weighted average helical twisting power before light irradiation is 0.05 μm -1 More preferably, 0.05 to 10.0 μm -1 More preferably, 0.1 to 10.0 μm -1 is more preferred.

[0114] [Step 5] In step 5, after step 4, the composition layer is subjected to a curing treatment to fix the alignment state of the liquid crystal compound, and a first optically anisotropic layer and a second optically anisotropic layer are formed. By carrying out this step, the alignment state of the liquid crystal compound in the composition layer is fixed, and as a result, a predetermined optically anisotropic layer is formed. In other words, a laminated film of an optically anisotropic layer in which a twisted aligned liquid crystal compound is fixed and an optically anisotropic layer in which a non-twisted aligned liquid crystal compound is fixed can be formed by a single coating treatment.

[0115] The method of the curing treatment is not particularly limited, and examples thereof include photocuring treatment and heat curing treatment. Among them, photoirradiation treatment is preferred, and ultraviolet irradiation treatment is more preferred. For ultraviolet irradiation, a light source such as an ultraviolet lamp is used. The amount of light (e.g., ultraviolet light) applied is not particularly limited, but is generally 100 to 800 mJ / cm 2 degree is preferred.

[0116] <Third embodiment> A third embodiment of the circularly polarizing plate of the present invention will be described with reference to the drawings. Fig. 12 shows a schematic cross-sectional view of the third embodiment of the optical film of the present invention. The circular polarizing plate 100C has a polarizer 10, a fourth optically anisotropic layer 24, and a third optically anisotropic layer 22 in this order. The third optically anisotropic layer 22 and the fourth optically anisotropic layer 24 are layers formed by fixing a rod-shaped liquid crystal compound LC that is twisted and aligned with the thickness direction as the helical axis. The molecular axis of the rod-shaped liquid crystal compound LC in the third optically anisotropic layer 22 is horizontal to the surface of the third optically anisotropic layer 22, and the molecular axis of the rod-shaped liquid crystal compound LC in the fourth optically anisotropic layer 24 is horizontal to the surface of the fourth optically anisotropic layer 24. In the circular polarizing plate 100C, the optically anisotropic layer formed using the liquid crystal compound includes the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24. That is, in the circular polarizing plate 100C, the optically anisotropic layer has a multilayer structure. Each layer will be described in detail below. Note that the polarizer 10 is the same as the polarizer 10 described in the first embodiment above, and therefore a description thereof will be omitted. Each layer will be described in detail below.

[0117] (Third optically anisotropic layer 22) As shown in FIG. 12, the third optically anisotropic layer 22 is a layer in which a rod-shaped liquid crystal compound LC is fixed, which is twisted and aligned with the thickness direction (z-axis direction in FIG. 12) as the helical axis, and the molecular axis of the rod-shaped liquid crystal compound LC in the third optically anisotropic layer is horizontal to the surface of the third optically anisotropic layer. The third optically anisotropic layer 22 is preferably a layer in which a chiral nematic phase having a so-called helical structure is fixed. In other words, the third optically anisotropic layer 22 is preferably a layer in which a liquid crystal compound is twisted and aligned with the thickness direction as the helical axis, and whose molecular axis is aligned horizontally is fixed. In addition, when forming the above phase, it is preferable to use a mixture of a liquid crystal compound exhibiting a nematic liquid crystal phase and a chiral agent described later. The meaning of the "fixed" state is as described above. The molecular axis being parallel to the surface of the optically anisotropic layer is defined as described in the first embodiment above.

[0118] The twist angle of the rod-shaped liquid crystal compound LC (the twist angle of the alignment direction of the rod-shaped liquid crystal compound LC) is preferably 78.6±10.0°, that is, the twist angle is preferably 68.6 to 88.6°. Among them, in terms of better effects of the present invention, the twist angle is more preferably 70.6 to 86.6°, and further preferably 72.6 to 84.6°. The liquid crystal compound being twisted means that the liquid crystal compound is twisted from one main surface to the other main surface of the third optically anisotropic layer 22 around the axis in the thickness direction of the third optically anisotropic layer 22. Accordingly, the orientation direction (in-plane slow axis direction) of the liquid crystal compound differs depending on the position in the thickness direction of the third optically anisotropic layer 22. 12, the right twist means that when observed from the polarizer 10 toward the third optically anisotropic layer 22, the in-plane slow axis of the third optically anisotropic layer 22 on the opposite side to the polarizer 10 side is positioned clockwise with respect to the in-plane slow axis of the third optically anisotropic layer 22 on the polarizer 10 side, which serves as the reference axis.

[0119] The torsion angle is measured using an AxoScan (polarimeter) device manufactured by Axometrics Inc. and the device analysis software of the same company.

[0120] It is preferable that the value of the product Δn3d3 of the refractive index anisotropy Δn3 of the third optically anisotropic layer 22 measured at a wavelength of 550 nm and the thickness d3 of the third optically anisotropic layer 22 satisfy the relationship of formula (3) in terms of better effects of the present invention. Formula (3) 110nm≦Δn3d3≦170nm Among these, it is more preferable that the relationship of formula (3A) is satisfied, and it is even more preferable that the relationship of formula (3B) is satisfied. Formula (3A) 120nm≦Δn3d3≦160nm Formula (3B) 130nm≦Δn3d3≦150nm The above Δn3d3 is measured using an AxoScan (polarimeter) device manufactured by Axometrics Inc. and the device analysis software of the same company, in the same manner as in the measurement of the torsion angle.

[0121] (Fourth optically anisotropic layer 24) As shown in FIG. 12, the fourth optically anisotropic layer 24 is a layer in which a rod-shaped liquid crystal compound LC is fixed, which is twisted and aligned with the thickness direction (z-axis direction in FIG. 12) as the helical axis, and the molecular axis of the rod-shaped liquid crystal compound LC in the fourth optically anisotropic layer is horizontal to the surface of the fourth optically anisotropic layer. The fourth optically anisotropic layer 24 is preferably a layer in which a chiral nematic phase having a so-called helical structure is fixed. In other words, the fourth optically anisotropic layer 24 is preferably a layer in which a liquid crystal compound is twisted and aligned with the thickness direction as the helical axis, and whose molecular axis is aligned horizontally is fixed. In addition, when forming the above phase, it is preferable to use a mixture of a liquid crystal compound exhibiting a nematic liquid crystal phase and a chiral agent described later. The meaning of the "fixed" state is as described above. The molecular axis being parallel to the surface of the optically anisotropic layer is defined as described in the first embodiment above.

[0122] The twist angle of the rod-shaped liquid crystal compound LC (the twist angle of the alignment direction of the rod-shaped liquid crystal compound LC) is preferably within a range of 26.5±10.0°. That is, the twist angle is preferably 16.5 to 36.5°. Among them, in terms of better effects of the present invention, the twist angle is more preferably 18.5 to 34.5°, and even more preferably 20.5 to 32.5°. The liquid crystal compound being twisted means that the liquid crystal compound is twisted from one main surface to the other main surface of the fourth optically anisotropic layer 24 around the axis in the thickness direction of the fourth optically anisotropic layer 24. Accordingly, the orientation direction (in-plane slow axis direction) of the liquid crystal compound differs depending on the position in the thickness direction of the fourth optically anisotropic layer 24. 12, the right twist means that when observed from the polarizer 10 toward the fourth optically anisotropic layer 24, the in-plane slow axis of the fourth optically anisotropic layer 24 on the side opposite to the polarizer 10 side is positioned clockwise with respect to the in-plane slow axis of the fourth optically anisotropic layer 24 on the polarizer 10 side, which serves as the reference axis.

[0123] It is preferable that the value of the product Δn4d4 of the refractive index anisotropy Δn4 of the fourth optically anisotropic layer 24 measured at a wavelength of 550 nm and the thickness d4 of the fourth optically anisotropic layer 24 satisfy the relationship of formula (4) in terms of better effects of the present invention. Formula (4) 252nm≦Δn4d4≦312nm Among these, it is more preferable that the relationship of formula (4A) is satisfied, and it is even more preferable that the relationship of formula (4B) is satisfied. Formula (4A) 262nm≦Δn4d4≦302nm Formula (4B) 272nm≦Δn4d4≦292nm The above Δn4d4 is measured using an AxoScan (polarimeter) device manufactured by Axometrics, Inc., using the device analysis software of the same company.

[0124] The in-plane slow axis of the third optically anisotropic layer 22 on the surface facing the fourth optically anisotropic layer 24 is parallel to the in-plane slow axis of the fourth optically anisotropic layer 24 on the surface facing the third optically anisotropic layer 22. The definition of parallel is as described above. That is, the angle formed by the in-plane slow axis of the third optically anisotropic layer 22 on the surface facing the fourth optically anisotropic layer 24 and the in-plane slow axis of the fourth optically anisotropic layer 24 on the surface facing the third optically anisotropic layer 22 is within 10° (0 to 10°).

[0125] The twist direction of the liquid crystal compound in the third optically anisotropic layer 22 and the twist direction of the liquid crystal compound in the fourth optically anisotropic layer 24 are preferably the same direction. For example, when the circular polarizing plate 100C is observed from the polarizer 10 side, if the in-plane slow axis of the third optically anisotropic layer 22 rotates clockwise based on the in-plane slow axis of the surface of the third optically anisotropic layer 22 opposite the fourth optically anisotropic layer 24, it is preferable that the in-plane slow axis of the surface of the fourth optically anisotropic layer 24 opposite the third optically anisotropic layer 22 rotates clockwise based on the in-plane slow axis of the surface of the fourth optically anisotropic layer 24 opposite the third optically anisotropic layer 22. Furthermore, when the circular polarizing plate 100C is observed from the polarizer 10 side, if the in-plane slow axis of the third optically anisotropic layer 22 rotates counterclockwise based on the in-plane slow axis of the surface of the third optically anisotropic layer 22 opposite the fourth optically anisotropic layer 24, it is preferable that the in-plane slow axis of the surface of the fourth optically anisotropic layer 24 opposite the third optically anisotropic layer 22 rotates counterclockwise based on the in-plane slow axis of the surface of the fourth optically anisotropic layer 24 opposite the third optically anisotropic layer 22.

[0126] An alignment film, which will be described later, may be disposed between the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24, but it is preferable that the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24 are adjacent to each other and there is substantially no alignment film between the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24, as shown in Fig. 12. When there is substantially no alignment film between the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24, the covalent bonds between the compounds contained in each optically anisotropic layer can be utilized, resulting in more excellent adhesion.

[0127] In FIG. 12, the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24 are formed using rod-like liquid crystal compounds, but the present invention is not limited to this embodiment. The liquid crystal compound may be the liquid crystal compound described in the first embodiment.

[0128] The third optically anisotropic layer 22 and the fourth optically anisotropic layer 24 are more preferably formed using a liquid crystal compound having a polymerizable group and reverse wavelength dispersion, since this can reduce changes in temperature or humidity. That is, the third optically anisotropic layer 22 or the fourth optically anisotropic layer 24 is preferably a layer formed by fixing a liquid crystal compound having a reverse wavelength dispersion property and a polymerizable group by polymerization or the like. The type of polymerizable group is not particularly limited, and is preferably a functional group capable of an addition polymerization reaction, more preferably a polymerizable ethylenically unsaturated group or a ring-polymerizable group, further preferably a (meth)acryloyl group, a vinyl group, a styryl group, or an allyl group, and particularly preferably a (meth)acryloyl group.

[0129] In the circular polarizing plate 100C, the relationship between the absorption axis of the polarizer 10 and the in-plane slow axes of the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24 preferably satisfies the following requirement (Xb) or (Yb). (Xb) The angle between the in-plane slow axis of the surface of the fourth optically anisotropic layer 24 facing the polarizer 10 and the absorption axis of the polarizer 10 is within the range of 0±10° (−10 to 10°) (preferably within the range of 0±6°). (Yb) The angle between the in-plane slow axis of the surface of the fourth optically anisotropic layer 24 facing the polarizer 10 and the absorption axis of the polarizer 10 is within the range of 90±10° (80 to 100°) (preferably within the range of 90±6°). As described above, the in-plane slow axis of the surface of the third optically anisotropic layer 22 facing the fourth optically anisotropic layer 24 is parallel to the in-plane slow axis of the surface of the fourth optically anisotropic layer 24 facing the third optically anisotropic layer 22.

[0130] The relationship between the absorption axis of the polarizer 10, the in-plane slow axis of the fourth optically anisotropic layer 24, and the in-plane slow axis of the third optically anisotropic layer 22 in the requirement represented by (Xb) above will be described in more detail with reference to FIG. 13. The arrow in the polarizer 10 in Fig. 13 indicates the absorption axis, and the arrows in the fourth optically anisotropic layer 24 and the third optically anisotropic layer 22 indicate the in-plane slow axis in each layer. Fig. 14 also shows the relationship between the absorption axis of the polarizer 10, the in-plane slow axis of the fourth optically anisotropic layer 24, and the in-plane slow axis of the third optically anisotropic layer 22 when observed from the white arrow in Fig. 13. 14, the rotation angle of the in-plane slow axis is expressed as a positive value in the counterclockwise direction and a negative value in the clockwise direction with respect to the absorption axis of polarizer 10 when observed from the white arrow in FIG.

[0131] 13, the absorption axis of the polarizer 10 and the in-plane slow axis of the surface 241 of the fourth optically anisotropic layer 24 facing the polarizer 10 are parallel to each other. The definition of "parallel" is as described above. That is, the angle between the absorption axis of the polarizer 10 and the in-plane slow axis of the surface 241 of the fourth optically anisotropic layer 24 facing the polarizer 10 is 0±10°. As described above, the fourth optically anisotropic layer 24 is a layer in which liquid crystal compounds are fixed in a twisted orientation with the thickness direction as the helical axis. Therefore, as shown in FIG. 13, the in-plane slow axis at the surface 241 on the polarizer 10 side of the fourth optically anisotropic layer 24 and the in-plane slow axis at the surface 221 on the third optically anisotropic layer 22 side of the fourth optically anisotropic layer 24 form the above-mentioned twist angle (26.5° in FIG. 13). That is, the in-plane slow axis of the fourth optically anisotropic layer 24 rotates by −26.5° (26.5° clockwise). Therefore, the angle φ2b between the absorption axis of the polarizer 10 and the in-plane slow axis at the surface 242 of the fourth optically anisotropic layer 24 is 26.5°. In addition, in Figure 13, the in-plane slow axis at surface 242 of the fourth optical anisotropic layer 24 is shown rotated 26.5° clockwise relative to the in-plane slow axis at surface 241 of the fourth optical anisotropic layer 24, but this is not limited to this embodiment, and the rotation angle may be in the range of 26.5±10.0° clockwise.

[0132] 13, the in-plane slow axis of the fourth optically anisotropic layer 24 at the surface 242 facing the third optically anisotropic layer 22 is parallel to the in-plane slow axis of the third optically anisotropic layer 22 at the surface 221 facing the fourth optically anisotropic layer 24. In other words, the angle φ3b between the absorption axis of the polarizer 10 and the in-plane slow axis of the third optically anisotropic layer 22 at the surface 221 facing the fourth optically anisotropic layer 24 is approximately the same as the angle φ2b.

[0133] As described above, the third optically anisotropic layer 22 is a layer in which a liquid crystal compound is fixed that is twisted and aligned with the thickness direction as the helical axis. Therefore, as shown in FIG. 13, the in-plane slow axis at the surface 221 of the third optically anisotropic layer 22 on the fourth optically anisotropic layer 24 side and the in-plane slow axis at the surface 222 of the third optically anisotropic layer 22 opposite to the fourth optically anisotropic layer 24 side form the above-mentioned twist angle (78.6° in FIG. 4). That is, the in-plane slow axis of the third optically anisotropic layer 22 rotates by −78.6° (78.6° clockwise). Therefore, the angle φ4b between the absorption axis of the polarizer 10 and the in-plane slow axis at the surface 222 of the third optically anisotropic layer 22 is 105.1°. In addition, in Figure 13, the in-plane slow axis at surface 222 of the third optical anisotropic layer 22 is shown rotated 78.6° clockwise relative to the in-plane slow axis at surface 221 of the third optical anisotropic layer 22, but this is not limited to this embodiment, and the rotation angle may be in the range of 78.6±10.0° clockwise.

[0134] As described above, in the embodiment of FIG. 13, the twist directions of the liquid crystal compounds in the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24 both show a clockwise (right-handed) twist with respect to the absorption axis of the polarizer 10. Although the embodiment in which the twist direction is clockwise (right-handed) has been described in detail in FIG. 13, the twist directions of the liquid crystal compounds in the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24 may both be counterclockwise.

[0135] Next, the relationship between the absorption axis of the polarizer 10 in the embodiment represented by (Yb) above, the in-plane slow axis of the third optically anisotropic layer 22, and the in-plane slow axis of the fourth optically anisotropic layer 24 will be described in more detail with reference to Figure 15. The arrow in the polarizer 10 in Fig. 15 indicates the absorption axis, and the arrows in the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24 indicate the in-plane slow axis in each layer. Fig. 16 also shows the relationship between the absorption axis of the polarizer 10, the in-plane slow axis at the surfaces 221 and 222 of the third optically anisotropic layer 22, and the in-plane slow axis at the surfaces 241 and 242 of the fourth optically anisotropic layer 24, when observed from the white arrows in Fig. 15. In Figure 16, when observed from the white arrow in Figure 15, the rotation angle of the in-plane slow axis is represented by a positive angle value in the counterclockwise direction and a negative angle value in the clockwise direction with the absorption axis of polarizer 10 as the reference (0°).

[0136] The embodiment shown in FIG. 15 has the same configuration as the embodiment shown in FIG. 13, except that the absorption axis of the polarizer 10 differs by 90° from the absorption axis of the polarizer 10 in FIG. 15, the absorption axis of the polarizer 10 is perpendicular to the in-plane slow axis at the surface 241 of the fourth optically anisotropic layer 24. That is, the angle φ1b between the absorption axis of the polarizer 10 and the in-plane slow axis at the surface 241 of the fourth optically anisotropic layer 24 is 90°. The definition of perpendicular is as described above. The in-plane slow axis at the surface 241 of the fourth optically anisotropic layer 24 facing the polarizer 10 and the in-plane slow axis at the surface 242 of the fourth optically anisotropic layer 24 facing the third optically anisotropic layer 22 form the above-mentioned twist angle (26.5° in FIG. 15). That is, the in-plane slow axis of the fourth optically anisotropic layer 24 rotates by −26.5° (26.5° clockwise). Therefore, the angle φ2b between the absorption axis of the polarizer 10 and the in-plane slow axis at the surface 242 of the fourth optically anisotropic layer 24 is 116.5°. In addition, in Figure 15, an embodiment is shown in which the in-plane slow axis at surface 242 of the fourth optical anisotropic layer 24 is rotated 26.5° clockwise relative to the in-plane slow axis at surface 241 of the fourth optical anisotropic layer 24, but this is not limited to this embodiment, and the rotation angle may be in the range of 26.5±10° clockwise.

[0137] 15, the in-plane slow axis of the fourth optically anisotropic layer 24 at the surface 242 facing the third optically anisotropic layer 22 is parallel to the in-plane slow axis of the third optically anisotropic layer 22 at the surface 221 facing the fourth optically anisotropic layer 24. In other words, the angle φ3b between the absorption axis of the polarizer 10 and the in-plane slow axis of the third optically anisotropic layer 22 at the surface 221 facing the fourth optically anisotropic layer 24 is approximately the same as the above-mentioned φ2b.

[0138] The in-plane slow axis at the surface 221 of the third optically anisotropic layer 22 facing the fourth optically anisotropic layer 24 and the in-plane slow axis at the surface 222 of the third optically anisotropic layer 22 facing the opposite side to the fourth optically anisotropic layer 24 form the above-mentioned twist angle (78.6° in FIG. 15). That is, the in-plane slow axis of the third optically anisotropic layer 22 rotates by −78.6° (78.6° clockwise). Therefore, the angle φ4b between the absorption axis of the polarizer 10 and the in-plane slow axis at the surface 222 of the third optically anisotropic layer 22 is 195.1°. In addition, in Figure 15, an embodiment is shown in which the in-plane slow axis at surface 222 of the third optical anisotropic layer 22 is rotated 78.6° clockwise relative to the in-plane slow axis at surface 221 of the third optical anisotropic layer 22, but this is not limited to this embodiment, and the rotation angle may be in the range of 78.6±10° clockwise.

[0139] As described above, in the embodiment of FIG. 15, the twist directions of the liquid crystal compounds in the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24 both show a clockwise (right-handed) twist with respect to the absorption axis of the polarizer 10. Although the embodiment in which the twist direction is clockwise (right-handed) has been described in detail in FIG. 15, the twist directions of the liquid crystal compounds in the third optically anisotropic layer 22 and the fourth optically anisotropic layer 24 may both be counterclockwise. Of the embodiment shown in FIG. 13 (requirement (Xb)) and the embodiment shown in FIG. 15 (requirement (Yb)), the embodiment shown in FIG. 13 is more preferable.

[0140] (other layers) The circularly polarizing plate 100C may have layers other than the polarizer 10, the third optically anisotropic layer 22, and the fourth optically anisotropic layer . The circular polarizing plate 100C may have a support. The form of the support is as described in the above-mentioned first embodiment. The circular polarizing plate 100C may have a support between the polarizer 10 and the third optically anisotropic layer 22. The circularly polarizing plate 100C may have an alignment film. The aspect of the alignment film is as explained in the first embodiment. The circularly polarizing plate 100C may have a pressure-sensitive adhesive layer. In particular, the third optically anisotropic layer 22 may have a pressure-sensitive adhesive layer on the surface opposite to the polarizer 10. As the pressure-sensitive adhesive constituting the pressure-sensitive adhesive layer, a known pressure-sensitive adhesive is used.

[0141] (Manufacturing method) The method for producing the circularly polarizing plate is not particularly limited, and may be a known method. The circularly polarizing plate may be produced continuously by roll-to-roll production. For example, a circular polarizing plate can be manufactured by preparing a third optically anisotropic layer and a fourth optically anisotropic layer each exhibiting a predetermined optical property, and bonding the optically anisotropic layers and the polarizer together in a predetermined order via an adhesive layer (e.g., a pressure-sensitive adhesive layer or an adhesive layer). Alternatively, a third optically anisotropic layer and a fourth optically anisotropic layer may be sequentially formed on a support using a polymerizable liquid crystal composition to produce an optical film, and the optical film obtained may be laminated to a polarizer to produce a circularly polarizing plate. For example, a polymerizable liquid crystal composition may be applied on a support to form a fourth optically anisotropic layer, and then a polymerizable liquid crystal composition may be applied on the fourth optically anisotropic layer to form a third optically anisotropic layer. The form of the polymerizable liquid crystal composition and the procedure of the method for producing an optically anisotropic layer using the polymerizable liquid crystal composition are as described in the first embodiment.

[0142] <Display device> The display device of the present invention includes a display element and the above-mentioned circularly polarizing plate. Usually, the optically anisotropic layer in the circularly polarizing plate is disposed on the display element side. In other words, the polarizer in the circularly polarizing plate is disposed on the viewing side. Examples of the display element include an organic EL display element and a liquid crystal display element. For example, an organic EL display device includes at least an organic EL display element and a circular polarizer. The circular polarizer is disposed so that the optically anisotropic layer faces the organic EL display element.

[0143] An organic EL display element is a member in which a light-emitting layer or a plurality of organic compound thin films including a light-emitting layer are formed between a pair of electrodes, an anode and a cathode, and may have a hole injection layer, a hole transport layer, an electron injection layer, an electron transport layer, a protective layer, etc. in addition to the light-emitting layer, and each of these layers may have other functions. Various materials can be used to form each layer. EXAMPLES

[0144] The features of the present invention will be described in more detail below with reference to examples and comparative examples. The materials, amounts, ratios, processing contents, and processing procedures shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the specific examples shown below.

[0145] <Example A1> (Preparation of Cellulose Acylate Film (Substrate)) The following components were put into a mixing tank, stirred, heated at 90°C for 10 minutes, and then filtered through a filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm to produce a cellulose acylate dope (hereinafter, also simply referred to as "dope"). The solid content of the obtained dope was 23.5% by mass, and the mass ratio of the solvent was methylene chloride / methanol / butanol = 81 / 18 / 1.

[0146] ---------------------------------------------------------------------------------- Cellulose Acylate Dope ---------------------------------------------------------------------------------- Cellulose acylate (acetyl substitution degree 2.86, viscosity average polymerization degree 310) 100 parts by mass Sugar ester compound 1 (shown in chemical formula (S4)) 6.0 parts by mass Sugar ester compound 2 (shown in chemical formula (S5)) 2.0 parts by mass Silica particle dispersion (AEROSIL R972, Nippon Aerosil Co., Ltd.) 0.1 part by mass Solvent (methylene chloride / methanol / butanol) specified amount ----------------------------------------------------------------------------------

[0147] [ka] JPEG0007578692000004.jpg4569

[0148] The above-mentioned dope was cast using a drum film-casting machine. The above-mentioned dope for forming the core layer and the above-mentioned dope for forming the surface layer on the core layer were co-cast from a die so as to be in contact with a metal substrate cooled to 0°C, and then the obtained film was peeled off. The drum was made of SUS (Steel Use Stainless).

[0149] The film peeled off from the drum was dried at 30 to 40°C for 20 minutes while being transported using a tenter device that clips both ends of the film with clips. Next, the obtained film was post-dried by zone heating while being transported with a roll. After that, the obtained film was knurled and then wound up. The thickness of the obtained long cellulose acylate film was 40 μm, Re(550) was 1 nm, and Rth(550) was 26 nm.

[0150] (Formation of Optically Anisotropic Layer) The cellulose acylate film prepared above was continuously subjected to a rubbing treatment, in such a manner that the longitudinal direction of the long film was parallel to the transport direction and the angle between the longitudinal direction of the film (transport direction) and the rotation axis of the rubbing roller was 90°. The following optically anisotropic layer coating solution (A) was applied onto the above-mentioned rubbed film using a Giesser coater, and heated for 60 seconds at 80° C. Thereafter, in a nitrogen atmosphere, the film on which the coating was formed was irradiated with light from a metal halide lamp (manufactured by Eye Graphics Co., Ltd.) at an irradiation dose of 500 mJ at 80° C. to fix the alignment state of the liquid crystal compound, thereby producing an optically anisotropic layer A1. The product Δnd of Δn and d of the optically anisotropic layer A1 at a wavelength of 550 nm was 200 nm, the direction of the in-plane slow axis on the surface of the optically anisotropic layer A1 facing the cellulose acylate film was 90°, and the direction of the in-plane slow axis on the surface of the optically anisotropic layer A1 opposite to the cellulose acylate film was 154° (twist angle = 64°). The direction of the in-plane slow axis is expressed as a positive value in the counterclockwise direction with the width direction of the cellulose acylate film as the reference (0°) when observing the laminate of the cellulose acylate film and the optically anisotropic layer A1 from the cellulose acylate film side. In addition, the molecular axis of the liquid crystal compound was parallel to the surface of the cellulose acylate film (or the surface of the optically anisotropic layer).

[0151] Composition of coating solution (A) for optically anisotropic layer ---------------------------------------------------------------------------------- 40 parts by weight of the following rod-shaped liquid crystal compound (A): 40 parts by weight of the following rod-shaped liquid crystal compound (B) 20 parts by weight of the following rod-shaped liquid crystal compound (C): Ethylene oxide modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 4 parts by mass Photopolymerization initiator (Irgacure 819, manufactured by Ciba Japan) 3 parts by weight 0.46 parts by weight of the following chiral agent (A): 0.5 parts by weight of the following polymerizable polymer (X): 0.1 parts by weight of the following polymer (A): Methyl isobutyl ketone 325 parts by weight ----------------------------------------------------------------------------------

[0152] Rod-shaped liquid crystal compound (A)

[0153] [ka]

[0154] Rod-shaped liquid crystal compound (B)

[0155] [ka]

[0156] Rod-shaped liquid crystal compound (C) (hereinafter referred to as a mixture of liquid crystal compounds)

[0157] [ka]

[0158] Chiral Agent (A)

[0159] [ka]

[0160] Polymerizable polymer (X)

[0161] [ka]

[0162] Polymer (A)

[0163] [ka]

[0164] (Preparation of circular polarizing plate) A polyvinyl alcohol (PVA) film with a thickness of 80 μm was dyed by immersing it in an aqueous iodine solution with an iodine concentration of 0.05% by mass at 30° C. for 60 seconds, and then stretched longitudinally to 5 times its original length while immersed in an aqueous boric acid solution with a boric acid concentration of 4% by mass for 60 seconds. The film was then dried at 50° C. for 4 minutes to obtain a polarizer with a thickness of 20 μm. A commercially available cellulose acylate film "TD80UL" (manufactured by Fujifilm Corporation) was prepared and immersed in a 1.5 mol / L aqueous solution of sodium hydroxide at 55°C, and then the sodium hydroxide was thoroughly washed off with water. Then, the film was immersed in a 0.005 mol / L aqueous solution of dilute sulfuric acid at 35°C for 1 minute, and then immersed in water to thoroughly wash off the dilute sulfuric acid. Finally, the sample was thoroughly dried at 120°C to prepare a polarizer protective film.

[0165] The polarizer protective film prepared above was attached to one side of the polarizer prepared above with a polyvinyl alcohol-based adhesive to prepare a laminate including a polarizer and a polarizer protective film disposed on one side of the polarizer.

[0166] An adhesive (SK-2057, manufactured by Soken Chemical & Engineering Co., Ltd.) was applied to the polarizer (without the polarizer protective film) side of the laminate prepared above to form an adhesive layer, and the prepared cellulose acylate film and the film having the optically anisotropic layer A1 were laminated together so that the adhesive layer and the cellulose acylate film were in close contact with each other. The absorption axis of the polarizer and the in-plane slow axis of the surface of the optically anisotropic layer A1 on the polarizer side were parallel to each other. Next, a pressure-sensitive adhesive was applied to the optically anisotropic layer A1 in the obtained laminate to form a pressure-sensitive adhesive layer. By the above procedure, a long circularly polarizing plate A1 in which a polarizer, a cellulose acylate film, an optically anisotropic layer A, and a pressure-sensitive adhesive layer were arranged in this order was produced.

[0167] <Examples A2 to A15> Circular polarizing plates A2 to A15 were produced according to the same procedure as in Example A1, except that the amount of chiral agent used and the thickness of the optically anisotropic layer were adjusted to obtain the retardation and twist angle shown in Table 1, and the rubbing axis angle and the like were adjusted to obtain the axial relationship of each layer shown in Table 1. The molecular axis of the liquid crystal compound in the optically anisotropic layer in each of the circular polarizing plates A2 to A15 was parallel to the surface of the optically anisotropic layer.

[0168] <Comparative Example A1> A circularly polarizing plate AC1 was prepared according to the same procedure as in Example A1, except that no chiral agent was used, the thickness of the optically anisotropic layer was adjusted to obtain the retardation shown in Table 1, and the rubbing axis angle and other factors were adjusted to obtain the axial relationship of each layer shown in Table 1.

[0169] <Evaluation> A Samsung GALAXY S4 equipped with an organic EL panel (organic EL display element) was disassembled, and the touch panel with the circular polarizer was peeled off from the organic EL display device. The circular polarizers A1 to A15 or AC1 prepared above were then attached to the touch panel while preventing air from entering, to produce an organic EL display device. The organic EL display device with the circular polarizer prepared above was fixed to an SR-3 (manufactured by Topcon) at a 40° incline, and the reflectance (Y) and color (a * / b * ) was measured. In this case, the average reflectance (Y) at azimuth angles of 0 to 180° and a * / b * The fluctuation range of (Δa * / Δb * ) was calculated and the results are summarized in Table 1. The average reflectance (Y) was evaluated according to the following criteria: In practical use, it is preferably D or higher. A: Average reflectance (Y) is less than 1.00% B: Average reflectance (Y) is 1.00% or more and less than 1.50% C: Average reflectance (Y) is 1.50% or more and less than 2.00% D: Average reflectance (Y) is 2.00% or more and less than 7.00% E: Average reflectance (Y) is 7.00% or more In addition, Δa * The evaluation was made according to the following criteria. From a practical standpoint, A is preferable. A: Less than 25 B: 25 or more Also, Δb * The evaluation was made according to the following criteria. From a practical standpoint, A is preferable. A: Under 19 B: 19 or above

[0170] In Table 1, the "Axis [°]" in the "Polarizer" column indicates the position of the absorption axis of the polarizer, with positive values ​​in the counterclockwise direction relative to the width direction of the circular polarizer (0°) when observing the circular polarizer from the polarizer side. It represents the angle between the width direction (transport direction) of the circularly polarizing plate and the absorption axis of the polarizer. In Table 1, the "LC Dispersion" column indicates "reverse dispersion" when the liquid crystal compound used is a liquid crystal compound with reverse wavelength dispersion, and indicates "normal dispersion" when the liquid crystal compound used is a liquid crystal compound with normal wavelength dispersion. In Table 1, the "Initial axis [°]" column indicates the position of the in-plane slow axis on the polarizer-side surface of the optically anisotropic layer, with the counterclockwise direction being expressed as a positive value with the width direction of the circular polarizer as the reference (0°) when observing the circular polarizer from the polarizer side. In Table 1, the column "Δnd [nm]" indicates the product Δnd (nm) of Δn and d (thickness) of the optically anisotropic layer at a wavelength of 550 nm. In Table 1, the column "Twist angle [°]" indicates the twist angle (°) of the twisted liquid crystal compound. In Table 1, the column "Average Y [%]" indicates the average reflectance (Y) (%).

[0171] [Table 1]

[0172] As shown in Table 1, it was confirmed that the desired effects were obtained when the circular polarizing plate of the present invention (corresponding to the first embodiment) was used. In particular, by comparing Examples A1 to A5, A14, and A15, it was confirmed that when the twist angle of the liquid crystal compound was 54 to 74° (preferably 59 to 69°), the effect was more excellent. Furthermore, by comparing Examples A1, A6 to A9, A12, and A13, it was confirmed that the effect is better when the product Δnd of Δn and d at a wavelength of 550 nm of the optically anisotropic layer is in the range of 170 to 230 nm (preferably 180 to 220 nm, more preferably 190 to 210 nm). Moreover, from a comparison of Examples A1, A10 to A11, it was confirmed that the effect was more excellent when the angle between the absorption axis of the polarizer and the in-plane slow axis of the optically anisotropic layer was less than 5°.

[0173] <Example B1> The cellulose acylate film prepared above was continuously subjected to rubbing treatment. At this time, the longitudinal direction of the long film was parallel to the transport direction, and the angle between the longitudinal direction of the film (transport direction) and the rotation axis of the rubbing roller was 76°. The longitudinal direction of the film (transport direction) was set to 90°, and the counterclockwise direction was expressed as a positive value with the width direction of the cellulose acylate film as the reference (0°) when observed from the cellulose acylate film side, and the rotation axis of the rubbing roller was 14°. In other words, the position of the rotation axis of the rubbing roller was rotated 76° clockwise with the longitudinal direction of the cellulose acylate film as the reference.

[0174] An optically anisotropic layer coating solution (B) containing the following rod-shaped liquid crystal compound was applied onto the rubbed film using a Giesser coater, and heated at 80° C. for 60 seconds. Thereafter, the film was irradiated with light from a 365 nm LED lamp (manufactured by Acroedge Co., Ltd.) at an irradiation dose of 40 mJ at 40° C. in air, to fix the alignment state of the liquid crystal compound in the half region on the cellulose acylate film side in the coating film. Furthermore, after heating at 80°C for 10 seconds, the liquid crystal compound was fixed in half of the air side area of ​​the coating film by irradiating it with light from a metal halide lamp (manufactured by Eye Graphics Co., Ltd.) at 80°C with an irradiation dose of 500 mJ under a nitrogen atmosphere, thereby producing an optically anisotropic layer. The optically anisotropic layer is composed of two layers exhibiting different optical anisotropy, and the layer on the cellulose acylate film side in the optically anisotropic layer (second optically anisotropic layer) is a layer in which a liquid crystal compound with reverse wavelength dispersion is fixed in a homogeneous orientation, and the product Δnd of Δn and d at a wavelength of 550 nm of this layer is 198 nm, and the in-plane slow axis is 104°. The layer on the air side in the optically anisotropic layer (first optically anisotropic layer) is a layer in which a liquid crystal compound with reverse wavelength dispersion is fixed in a twisted orientation with the thickness direction as the helical axis, and the molecular axis of the liquid crystal compound in the layer is horizontal to the surface of the optically anisotropic layer, and the product Δnd of Δn and d at a wavelength of 550 nm of this layer is 191 nm, and the direction of the in-plane slow axis is 104° on the film side surface and 189° (twist angle = 85°) on the air side surface. The above angle is expressed as a positive value in the counterclockwise direction with the width direction of the cellulose acylate film as the reference (0°) when the optically anisotropic layer is observed from the cellulose acylate film side.

[0175] Composition of coating solution for optically anisotropic layer (B) ---------------------------------------------------------------------------------- 40 parts by weight of the above rod-shaped liquid crystal compound (A) 40 parts by weight of the above rod-shaped liquid crystal compound (B) 20 parts by weight of the above rod-shaped liquid crystal compound (C) Ethylene oxide modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 4 parts by mass Photopolymerization initiator (Irgacure 819, manufactured by Ciba Japan) 3 parts by weight 0.51 parts by weight of the chiral agent (A) 0.46 parts by mass of the following chiral agent (B) 0.5 parts by weight of the above polymerizable polymer (X) 0.1 parts by weight of the above polymer (A) Methyl isobutyl ketone 325 parts by weight ----------------------------------------------------------------------------------

[0176] (Chiral Agent B)

[0177] [ka]

[0178] (Preparation of circular polarizing plate) According to the method described in Example A1, a laminate including a polarizer and a polarizer protective film disposed on one side of the polarizer was prepared. An adhesive (SK-2057, manufactured by Soken Chemical Industries, Ltd.) was applied to the polarizer (without the polarizer protective film) side of the laminate prepared above to form an adhesive layer, and the cellulose acylate film prepared above and a film having an optically anisotropic layer were bonded together so that the adhesive layer and the cellulose acylate film were in close contact with each other. The absorption axis of the polarizer was bonded to the angle position shown in Table 2 below. Next, a pressure-sensitive adhesive was applied onto the optically anisotropic layer in the obtained laminate to form a pressure-sensitive adhesive layer. By the above procedure, a long circularly polarizing plate B1 was prepared in which a polarizer, a cellulose acylate film, an optically anisotropic layer, and a pressure-sensitive adhesive layer were arranged in this order.

[0179] <Examples B2 to B19> Circular polarizing plates B2 to B19 were produced according to the same procedure as in Example B1, except that the amount of chiral agent used and the thickness of the optically anisotropic layer were adjusted to obtain the retardation and twist angle as shown in Table 2, and the rubbing axis angle and the like were adjusted to obtain the axial relationship of each layer as shown in Table 2. In addition, the molecular axis of the liquid crystal compound in the first optically anisotropic layer in each of the circular polarizers A2 to A15 was parallel to the surface of the first optically anisotropic layer.

[0180] <Comparative Example B1> A circularly polarizing plate BC1 was prepared in the same manner as in Example B1, except that the rod-shaped liquid crystal compound (C) described above was used instead of the rod-shaped liquid crystal compounds (A) and (B), the amount of the chiral agent used and the thickness of the optically anisotropic layer were adjusted so as to obtain the retardation and twist angle shown in Table 2, and the rubbing axis angle and the like were adjusted so as to obtain the axial relationship of each layer shown in Table 2. In the circular polarizing plate BC1, a liquid crystal compound having normal wavelength dispersion was used as the liquid crystal compound.

[0181] The above-prepared circular polarizing plates B1 to B19 and BC1 were used to carry out the <Evaluation> carried out in the above-mentioned Example A1. The results are summarized in Table 2.

[0182] In Table 2, the "Axis [°]" in the "Polarizer" column indicates the position of the absorption axis of the polarizer, with positive values ​​in the counterclockwise direction relative to the width direction of the circular polarizer (0°) when observing the circular polarizer from the polarizer side. In Table 2, the "LC Dispersion" column indicates "reverse dispersion" when the liquid crystal compound used is a liquid crystal compound with reverse wavelength dispersion, and indicates "normal dispersion" when the liquid crystal compound used is a liquid crystal compound with normal wavelength dispersion. In Table 2, the column "Δnd [nm]" indicates the product Δnd (nm) of Δn and d (thickness) of the optically anisotropic layer at a wavelength of 550 nm. In Table 2, the "Initial axis [°]" column indicates the position of the in-plane slow axis on the polarizer-side surface of the optically anisotropic layer, with the counterclockwise direction being expressed as a positive value with the width direction of the circular polarizer as the reference (0°) when observing the circular polarizer from the polarizer side.

[0183] [Table 2]

[0184] As shown in Table 2, it was confirmed that the desired effects were obtained when the circular polarizing plate of the present invention (corresponding to the second embodiment) was used. In particular, by comparing Examples B1 to B5, B18 and B19, it was confirmed that the effect was superior when the twist angle of the liquid crystal compound in the first optically anisotropic layer was in the range of 75 to 95° (preferably 80 to 90°). Moreover, by comparing Examples B1, B6 to B9, B14 and B15, it was confirmed that a more excellent effect was obtained when the Δnd of the second optically anisotropic layer was in the range of 180 to 220 nm (preferably 190 to 210 nm). Moreover, by comparing Examples B10, B11, B16 and B17, it was confirmed that when the Δnd of the first optically anisotropic layer was in the range of 160 to 220 nm (preferably 170 to 210 nm), a more excellent effect was obtained. Furthermore, comparison of Examples B1, B12, and B13 confirmed that a more excellent effect was obtained when the angle between the absorption axis of the polarizer and the in-plane slow axis of the second optically anisotropic layer was in the range of 13±3°. [Explanation of symbols]

[0185] 10 Polarizer 12 Optically anisotropic layer 14 First optically anisotropic layer 16 Second optically anisotropic layer 18 Support 20 composition layer 20A 1st area 20B 2nd area 22 Third optically anisotropic layer 24 Fourth optically anisotropic layer 100A, 100B, 100C Circular polarizing plate

Claims

1. A circular polarizing plate having a polarizer and an optically anisotropic layer, the optically anisotropic layer is a layer in which a liquid crystal compound having reverse wavelength dispersion properties is fixed and twisted and aligned with a helical axis in the thickness direction; a molecular axis of the liquid crystal compound in the optically anisotropic layer is parallel to a surface of the optically anisotropic layer, The twist angle of the twisted liquid crystal compound is 64±20°, The optically anisotropic layer formed by using a liquid crystal compound includes only the optically anisotropic layer, A circularly polarizing plate, wherein a product Δnd of a refractive index anisotropy Δn of the optically anisotropic layer measured at a wavelength of 550 nm and a thickness d of the optically anisotropic layer is 160 to 240 nm.

2. A polarizer, a second optically anisotropic layer, and a first optically anisotropic layer in this order, the first optically anisotropic layer is a layer in which a liquid crystal compound having reverse wavelength dispersion is fixed and twisted and aligned with a helical axis in a thickness direction, a molecular axis of the liquid crystal compound in the first optically anisotropic layer is parallel to a surface of the first optically anisotropic layer, the second optically anisotropic layer is a layer in which a liquid crystal compound having a reverse wavelength dispersion property is fixed in a homogeneously aligned state, the twist angle in the first optically anisotropic layer is 85±20°; an in-plane slow axis of the first optically anisotropic layer at a surface facing the second optically anisotropic layer is parallel to an in-plane slow axis of the second optically anisotropic layer at a surface facing the first optically anisotropic layer, a value of a product Δn1d1 of a refractive index anisotropy Δn1 of the first optically anisotropic layer measured at a wavelength of 550 nm and a thickness d1 of the first optically anisotropic layer satisfies the relationship of formula (1), A circularly polarizing plate, wherein a value of a product Δn2d2 of a refractive index anisotropy Δn2 of the second optically anisotropic layer measured at a wavelength of 550 nm and a thickness d2 of the second optically anisotropic layer satisfies the relationship of formula (2). Formula (1) 150nm≦Δn1d1≦230nm Formula (2) 140nm≦Δn2d2≦220nm

3. 3. The circular polarizing plate according to claim 1, wherein the liquid crystal compound having reverse wavelength dispersion is a rod-shaped liquid crystal compound having reverse wavelength dispersion.

4. An organic electroluminescence display device comprising the circular polarizer according to any one of claims 1 to 3.

Citation Information

Patent Citations

  • Circularly polarizing plate, manufacturing method therefor, optical film, liquid crystal display device, and electroluminescence device

    JP2007003824A

  • Retardation plate for circularly polarizing plate, circularly polarizing plate, and organic el (electroluminescence) display device

    JP2014209219A

  • Retardation plate for circularly polarizing plate, circularly polarizing plate, and organic el (electroluminescence) display device

    JP2014209220A

  • Resin film, λ / 4 plate, circularly polarizing plate, organic electroluminescence display device, and manufacturing method

    JP2015111257A

  • Optical film

    JP2016528543A