Optical laminate and image display device
By establishing a specific relationship between adhesive and resin layer properties, the optical laminate addresses durability and reflection issues, ensuring stable performance under harsh conditions.
Patent Information
- Application Number
- JP2022553861
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-30
- Filing Date
- 2021-09-22
- Publication Date
- 2024-11-06
- Estimated Expiration
- 2041-09-22
AI Technical Summary
Optical laminates with photo-alignment layers experience uneven reflection and durability issues under high-temperature, high-humidity environments due to insufficient bonding and deformation of resin layers.
The optical laminate is designed with specific relationships between the storage elastic modulus of adhesive layers and the storage elastic modulus and moist heat strain of resin layers, ensuring that the laminate maintains structural integrity under harsh conditions.
The laminate exhibits enhanced durability and reduces uneven reflection, providing a stable optical performance in high-temperature, high-humidity environments.
Smart Images

Figure 0007578708000050 
Figure 0007578708000051 
Figure 0007578708000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical laminate and an image display device. [Background technology]
[0002] Optical films such as optical compensation sheets and retardation films are used in various image display devices from the viewpoints of eliminating image coloration and widening the viewing angle. Stretched birefringent films have been used as optical films, but in recent years, it has been proposed to use optically anisotropic layers using liquid crystal compounds in place of stretched birefringent films.
[0003] It is known that such an optically anisotropic layer has an alignment film provided on the support on which the optically anisotropic layer is formed in order to align the liquid crystal compound, and a photo-alignment film that has been subjected to a photo-alignment treatment instead of a rubbing treatment is also known as this alignment film.
[0004] For example, Patent Document 1 describes an optical laminate having a support, an alignment layer, a light absorption anisotropic layer, and an adhesive layer in that order, in which the alignment layer is a photoalignment layer formed using a composition for forming an alignment layer that contains a cinnamoyl compound having a functional group with an ethylenically unsaturated double bond ([Claim 1]). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2020 / 080359 Summary of the Invention [Problem to be solved by the invention]
[0006] The present inventors have produced an optical laminate having a layer structure in which the optical alignment layer and the optically absorbing anisotropic layer described in Patent Document 1 are sandwiched between two pressure-sensitive adhesive layers in order to attach the laminate to an image display element or the like, and have found that, depending on the type of optical alignment film, when the laminate is exposed to a high-temperature, high-humidity environment, uneven reflection from the surface may occur. In other words, it has been found that the durability to a high-temperature, high-humidity environment (hereinafter, "durability to a high-temperature, high-humidity environment" may be simply referred to as "durability") may be insufficient. Furthermore, the present inventors have clarified that the same phenomenon occurs in the above optical laminate even when the photo-alignment layer is changed to a simple resin layer.
[0007] Therefore, an object of the present invention is to provide an optical laminate having excellent durability and an image display device using the same. [Means for solving the problem]
[0008] As a result of intensive research to solve the above-mentioned problems, the inventors focused on one of the two adhesive layers contained in the optical laminate and the resin layer adjacent to it (e.g., a photo-alignment layer), and found that the above-mentioned problems can be solved when the storage modulus Ep of the adhesive layer and the storage modulus Ea and moist heat distortion δa of the resin layer satisfy a specific relationship, thereby completing the present invention. That is, the present inventors have found that the above object can be achieved by the following configuration.
[0009] [1] An optical laminate having, in this order, a pressure-sensitive adhesive layer 1, a specific laminate having a resin layer and a light absorption anisotropic layer adjacent to each other, and a pressure-sensitive adhesive layer 2, The light absorbing anisotropic layer contains a dichroic material, The pressure-sensitive adhesive layer 1 is adjacent to a resin layer of the specific laminate, An optical laminate, in which the storage modulus Ep of the pressure-sensitive adhesive layer 1, and the storage modulus Ea and the wet heat distortion Δa of the resin layer satisfy the following formula (1-1). 1 / 4(3×Ep / Ea) 2 / 3 > δa (1-1) However, the storage modulus Ep of the adhesive layer 1The unit is MPa, Unit of storage modulus Ea of resin layer is G The elastic modulus is expressed in Pa, and the wet heat distortion Δa of the resin layer is a value defined by the following formula (2). δa=L max / L0×100 (2) L max : Maximum displacement (mm) when the temperature profile in the following heat and humidity distortion test is applied L0: Distance between chucks in the following heat and humidity distortion test (mm) Humid heat distortion test: A single resin layer with a thickness of 10 μm was used as the test specimen, and with a chuck distance of 15 mm and a tensile load of 0.02 mN applied, it was held in an environment of 25°C and 50% relative humidity for 30 minutes, then the temperature and humidity were raised to 60°C and 90% relative humidity over 80 minutes, and then it was held in an environment of 60°C and 90% relative humidity for 120 minutes, after which the temperature and humidity were lowered to 25°C and 50% relative humidity over 80 minutes.
[0010] [2] The optical laminate according to [1], wherein the resin layer is an alignment layer. [3] The optical laminate according to [2], wherein the alignment layer is a photoalignment layer. [4] The optical laminate according to any one of [1] to [3], wherein the storage modulus Ep of the pressure-sensitive adhesive layer 1, and the storage modulus Ea and the moist heat distortion Δa of the resin layer satisfy the following formula (1-2): 1 / 4(3×Ep / Ea) 2 / 3 -δa ≧ 0.15 (1-2) [5] The optical laminate according to any one of [1] to [4], wherein the resin layer has a storage modulus Ea of 1 GPa or more and 10 GPa or less. [6] The optical laminate according to any one of [1] to [5], wherein the resin layer has a storage modulus Ea of 1 GPa or more and 5 GPa or less. [7] The optical laminate according to any one of [1] to [6], which has a thickness of 50 μm or less. [8] The optical laminate according to any one of [1] to [7], wherein the resin layer has a thickness of 2 μm or less. [9] An image display device comprising the optical laminate according to any one of [1] to [8] and an image display element.
[10] The image display device according to [9], which is an organic electroluminescence (EL) display device. Effect of the Invention
[0011] According to the present invention, it is possible to provide an optical laminate having excellent durability and an image display device using the same. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic cross-sectional view showing an example of the optical layered body of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of the optical layered body of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits. Furthermore, in this specification, parallel, orthogonal, horizontal, and vertical do not mean parallel, orthogonal, horizontal, and vertical in the strict sense, but rather mean a range of parallel ±10°, a range of orthogonal ±10°, horizontal ±10°, and vertical ±10°, respectively. In the present specification, each component may be used alone or in combination of two or more substances corresponding to each component. When two or more substances are used in combination for each component, the content of the component refers to the total content of the substances used in combination, unless otherwise specified. In addition, in this specification, "(meth)acrylate" is a notation representing "acrylate" or "methacrylate", "(meth)acryl" is a notation representing "acryl" or "methacryl", and "(meth)acryloyl" is a notation representing "acryloyl" or "methacryloyl".
[0014] [I] Optical laminate The optical laminate of the present invention (hereinafter also referred to as "the laminate of the present invention") is An optical laminate having, in this order, a pressure-sensitive adhesive layer 1, a specific laminate having a resin layer and a light absorption anisotropic layer adjacent to each other, and a pressure-sensitive adhesive layer 2, the light absorption anisotropic layer contains a dichroic material, The pressure-sensitive adhesive layer 1 is adjacent to the resin layer of the specific laminate, This is an optical laminate in which the storage modulus Ep of the pressure-sensitive adhesive layer 1, and the storage modulus Ea and the wet heat distortion Δa of the resin layer satisfy the formula (1-1) described below. Here, the state where the layers are adjacent to each other means that the layers are in direct contact with each other.
[0015] The inventors have discovered that when an optical laminate having a layer structure in which a resin layer and a specific laminate having optical absorption anisotropy adjacent to each other are sandwiched between two pressure-sensitive adhesive layers is exposed to a high-temperature, high-humidity environment, the resin layer deforms into a wrinkled shape, causing reflection unevenness. Therefore, in the optical laminate of the present invention, since there is a specific relationship between the storage modulus Ep of one of the pressure-sensitive adhesive layers and the storage modulus Ea and moist heat distortion δa of the adjacent resin layer, it is believed that the resin layer is unlikely to deform even when exposed to a high-temperature, high-humidity environment, or even if it does deform, it will not become wrinkled.
[0016] First, the laminate of the present invention will be described with reference to the drawings.
[0017] FIG. 1 is a schematic cross-sectional view showing an example of the laminate of the present invention. The optical laminate 100 shown in FIG. 1 has, in this order, a pressure-sensitive adhesive layer 1, a specific laminate 40 having a resin layer 20 and an optically absorptive anisotropic layer 30 adjacent to each other, and a pressure-sensitive adhesive layer 2. The light absorbing anisotropic layer 30 contains a dichroic material. The pressure-sensitive adhesive layer 1 is adjacent to the resin layer 20 of the specific laminate 40 . The storage modulus Ep of the pressure-sensitive adhesive layer 1, and the storage modulus Ea and the wet heat distortion Δa of the resin layer 20 satisfy the formula (1-1) described below.
[0018] FIG. 2 is a schematic cross-sectional view showing another example of the laminate of the present invention. The optical laminate 200 shown in FIG. 2 has, in this order, a λ / 4 plate 80, an adhesive layer 1, a specific laminate 42 having a photo-alignment layer 22 and an optically absorptive anisotropic layer 30 adjacent to each other, an adhesive layer 2, and a surface protection layer 70. The specific laminate 42 has a cured layer 50 on the surface of the optically absorptive anisotropic layer 30 opposite the optical alignment layer 22 , and has an oxygen barrier layer 60 on the surface of the cured layer 50 opposite the optically absorptive anisotropic layer 30 . The light absorbing anisotropic layer 30 contains a dichroic material. The pressure-sensitive adhesive layer 1 is adjacent to the photoalignment layer 22 of the specific laminate 42 . The optical laminate 200 also has a surface protective layer 70 on the surface of the pressure-sensitive adhesive layer 2 opposite the oxygen barrier layer 60 . The optical laminate 200 also has a λ / 4 plate 80 on the surface of the pressure-sensitive adhesive layer 1 opposite the optical alignment layer 22 . The storage modulus Ep of the pressure-sensitive adhesive layer 1, and the storage modulus Ea and the moist heat distortion Δa of the photoalignment layer 22 satisfy the formula (1-1) described below.
[0019] In the laminate of the present invention, the storage modulus Ep of the pressure-sensitive adhesive layer 1, and the storage modulus Ea and the wet heat distortion Δa of the photoalignment layer 22 satisfy the following formula (1-1). 1 / 4(3×Ep / Ea) 2 / 3 > δa (1-1)
[0020] However, the storage modulus Ep of the pressure-sensitive adhesive layer 1 The unit is MPa, Unit of storage elastic modulus Ea of the resin layer is GIt is Pa. Here, the storage elastic modulus Ep and the storage elastic modulus Ea are measured by a nanoindentation method. The storage modulus can be measured by the nanoindentation method, for example, using a nanoindenter (product name "Triboindenter TI-950", manufactured by Hysitron). In this measurement, the measurement mode is a single indentation measurement, the measurement temperature is 25°C, the indenter used is a cube corner indenter, the indenter indentation load on the measurement object is 20μN, the indenter indentation speed is 2μm / sec, and after creeping at 20μN for 5 seconds, the indenter is pulled out from the measurement object at a speed of 2μm / sec. The storage modulus based on the nanoindentation method is derived by the Oliver-Pharr method using the device used. A specific derivation method is as described, for example, in Hand book of Micro / nano Tribology (Second Edition) Edited by Bharat Bhushan, CRC Press (ISBN0-8493-8402-8). The storage modulus can be measured by nanoindentation either from the surface of the film or from the cross-sectional direction of the film. When measuring from the cross-sectional direction, reliable data can be obtained if the film thickness is 50 times or more the indentation depth.
[0021] On the other hand, the wet heat distortion Δa of the resin layer is a value defined by the following formula (2) and can be measured by thermomechanical analysis (TMA). As a thermomechanical analyzer, for example, a product name "TMA4000SE and temperature and humidity generating unit HC9700" (manufactured by Netzsch) can be used. δa=L max / L0×100 (2) L max : Maximum displacement (mm) when the temperature profile in the following heat and humidity distortion test is applied L0: Distance between chucks in the following heat and humidity distortion test Humid heat distortion test: A single resin layer with a thickness of 10 μm was used as the test specimen, and with a chuck distance of 15 mm and a tensile load of 0.02 mN applied, it was held in an environment of 25°C and 50% relative humidity for 30 minutes, then the temperature and humidity were raised to 60°C and 90% relative humidity over 80 minutes, and then it was held in an environment of 60°C and 90% relative humidity for 120 minutes, after which the temperature and humidity were lowered to 25°C and 50% relative humidity over 80 minutes.
[0022] In the present invention, for the reason that the durability of the optical laminate is further improved (hereinafter also referred to as "the reason that the effects of the present invention are superior"), it is preferable that the storage modulus Ep of the pressure-sensitive adhesive layer 1, and the storage modulus Ea and moist heat distortion Δa of the resin layer satisfy the following formula (1-2). 1 / 4(3×Ep / Ea) 2 / 3 -δa ≧ 0.15 (1-2)
[0023] The thickness of the laminate of the present invention is preferably 100 μm or less, and more preferably 50 μm or less, for reasons of excellent flexibility. The thickness of the laminate of the present invention is preferably 1 μm or more, and more preferably 10 μm or more.
[0024] Each layer of the laminate of the present invention will be described below.
[0025] [1] Adhesive layer 1 and adhesive layer 2 As described above, the laminate of the present invention has pressure-sensitive adhesive layer 1 and pressure-sensitive adhesive layer 2. Examples of adhesives contained in adhesive layer 1 and adhesive layer 2 include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, urethane-based adhesives, vinyl alkyl ether-based adhesives, polyvinyl alcohol-based adhesives, polyvinylpyrrolidone-based adhesives, polyacrylamide-based adhesives, and cellulose-based adhesives. Among these, from the viewpoints of transparency, weather resistance, heat resistance, and the like, acrylic adhesives (pressure-sensitive adhesives) are preferred.
[0026] The adhesive layer 1 and the adhesive layer 2 can be formed, for example, by a method in which a solution of an adhesive is applied onto a release sheet, dried, and then transferred to the surface of a transparent resin layer; a method in which a solution of an adhesive is directly applied to the surface of a transparent resin layer, and then dried; or the like. The adhesive solution is prepared, for example, as a solution of about 10 to 40 mass % by dissolving or dispersing the adhesive in a solvent such as toluene or ethyl acetate. Examples of the coating method that can be used include roll coating methods such as reverse coating and gravure coating, spin coating, screen coating, fountain coating, dipping, and spraying.
[0027] Examples of materials constituting the release sheet include suitable thin sheets such as synthetic resin films, such as polyethylene, polypropylene, and polyethylene terephthalate; rubber sheets; paper; cloth; nonwoven fabrics; nets; foam sheets; and metal foils.
[0028] [Adhesive layer thickness] The thickness of the pressure-sensitive adhesive layer 1 and the pressure-sensitive adhesive layer 2 is not particularly limited, but in order to obtain better effects of the present invention, the thickness is preferably 3 μm to 50 μm, more preferably 4 μm to 40 μm, and even more preferably 5 μm to 30 μm. For reasons why the effects of the present invention are superior, it is preferable that the thickness of at least one of adhesive layer 1 and adhesive layer 2 is thicker than the thickness of the specific laminate described below, and it is preferable that the thickness of both adhesive layer 1 and adhesive layer 2 is thicker than the thickness of the specific laminate described below.
[0029] [2] Specific laminate As described above, the laminate of the present invention includes a specific laminate having a resin layer and an optically absorptive anisotropic layer adjacent to each other. The specific laminate may include layers other than the resin layer and the optically absorptive anisotropic layer. Here, the pressure-sensitive adhesive layer 1 is, as described above, a pressure-sensitive adhesive layer adjacent to the resin layer of the specific laminate. In addition, the above-mentioned pressure-sensitive adhesive layer 2 is preferably adjacent to the light absorption anisotropic layer of the specific laminate (if the specific laminate has a cured layer or an oxygen barrier layer described below, these layers). In other words, the specific laminate is preferably a laminate consisting of all layers present between the pressure-sensitive adhesive layer 1 and the pressure-sensitive adhesive layer 2.
[0030] Each layer of the specific laminate will now be described.
[0031] [Resin layer] The resin layer contained in the specific laminate is not particularly limited, and various known resin layers can be used. Examples of the resin layer include a layer containing a liquid crystal compound, which is described below as an example of a cured layer, a layer obtained by curing a composition containing a polyfunctional monomer, and a layer obtained by curing a composition containing a polymer having a functional group. Another example of the resin layer is a layer made of a resin that is simply dried and solidified, such as a resin that is not polymerizable by itself (hereinafter, also referred to as a "resin binder"). Examples of such resin binders include epoxy resins, diallyl phthalate resins, silicone resins, phenolic resins, unsaturated polyester resins, polyimide resins, polyurethane resins, melamine resins, urea resins, ionomer resins, ethylene ethyl acrylate resins, acrylonitrile acrylate styrene copolymer resins, acrylonitrile styrene resins, acrylonitrile chlorinated polyethylene styrene copolymer resins, ethylene vinyl acetate resins, ethylene vinyl alcohol copolymer resins, acrylonitrile butadiene styrene copolymer resins, vinyl chloride resins, chlorinated polyethylene resins, polyvinylidene chloride resins, cellulose acetate resins, fluororesins, polyoxymethylene resins, polyamide resins, poly Examples of the resin include arylate resin, thermoplastic polyurethane elastomer, polyether ether ketone resin, polyether sulfone resin, polyethylene, polypropylene, polycarbonate resin, polystyrene, polystyrene-maleic acid copolymer resin, polystyrene-acrylic acid copolymer resin, polyphenylene ether resin, polyphenylene sulfide resin, polybutadiene resin, polybutylene terephthalate resin, acrylic resin, methacrylic resin, methylpentene resin, polylactic acid, polybutylene succinate resin, butyral resin, formal resin, polyvinyl alcohol, polyvinylpyrrolidone, ethyl cellulose, carboxymethyl cellulose, gelatin, and copolymer resins thereof. The function of such a resin layer is not particularly limited, and may be, for example, a layer having a function such as a stress relaxation layer, a protective layer, an alignment layer, a flattening layer, or a refractive index adjustment layer.
[0032] [Alignment Layer] The resin layer is preferably an alignment layer so as not to impede the alignment of the adjacent light absorptive anisotropic layer. Examples of the type of alignment layer include a photo-alignment layer, a rubbing treatment alignment layer, etc. Among these, a photo-alignment layer is preferred because it provides a superior effect of the present invention.
[0033] <Photoalignment layer> The photo-alignment layer is a layer to which an alignment control force is imparted by light irradiation.
[0034] Because the effect of the present invention is more excellent for the obtained optical laminate, the photo-alignment layer is preferably an alignment layer imparted with an alignment control force, obtained through a process of applying a composition containing a compound having a photoreactive group (photoactive compound) (hereinafter also abbreviated as "composition for forming a photo-alignment layer") onto a polymer film to form a coating film (coating film formation process), a process of drying the coating film by heating (drying process), and a process of irradiating the dried coating film with polarized light or unpolarized light obliquely to the coating film surface (light irradiation process). Hereinafter, "the effect of the present invention is more excellent with respect to the obtained optical layered body" will also be simply referred to as "the effect of the present invention is more excellent."
[0035] <Coating film formation process> As described above, the coating film forming step is a step of applying the photoalignment layer forming composition onto a polymer film to form a coating film.
[0036] (Polymer film) The polymer film is not particularly limited, and a commonly used polymer film (for example, a polarizer protective film) can be used. Specific examples of polymers that constitute the polymer film include cellulose-based polymers; acrylic-based polymers having acrylic acid ester polymers such as polymethyl methacrylate and lactone ring-containing polymers; thermoplastic norbornene-based polymers; polycarbonate-based polymers; polyester-based polymers such as polyethylene terephthalate and polyethylene naphthalate; styrene-based polymers such as polystyrene and acrylonitrile-styrene copolymers (AS resins); polyolefin-based polymers such as polyethylene, polypropylene, and ethylene-propylene copolymers; vinyl chloride-based polymers; amide-based polymers such as nylon and aromatic polyamides; imide-based polymers; sulfone-based polymers; polyethersulfone-based polymers; polyetheretherketone-based polymers; polyphenylene sulfide-based polymers; vinylidene chloride-based polymers; vinyl alcohol-based polymers; vinyl butyral-based polymers; arylate-based polymers; polyoxymethylene-based polymers; epoxy-based polymers; or mixtures of these polymers.
[0037] Of these, cellulose-based polymers (hereinafter also referred to as "cellulose acylate"), such as triacetyl cellulose, can be preferably used. In addition, from the viewpoint of processability and optical performance, it is also preferable to use an acrylic polymer. Examples of the acrylic polymer include polymethyl methacrylate and lactone ring-containing polymers described in paragraphs
[0017] to
[0107] of JP-A-2009-98605.
[0038] In the present invention, in an embodiment in which a polymer film that can be peeled off from the produced optical laminate is used, a cellulose-based polymer or a polyester-based polymer can be preferably used.
[0039] In the present invention, the polymer film is preferably transparent. Here, the term "transparent" in the present invention indicates that the transmittance of visible light is 60% or more, preferably 80% or more, and particularly preferably 90% or more.
[0040] The thickness of the polymer film is not particularly limited, but is preferably 40 μm or less because it allows the thickness of the optical laminate to be thin, etc. The lower limit is not particularly limited, but is usually 5 μm or more.
[0041] (photoactive compound) As described above, the photoalignment composition contains a compound having a photoreactive group (photoactive compound). A photoreactive group is a group that generates a liquid crystal alignment ability by irradiation with light. Specifically, it generates a photoreaction that is the origin of the liquid crystal alignment ability, such as an orientation induction or isomerization reaction, dimerization reaction, photocrosslinking reaction, or photodecomposition reaction of a molecule (called a photoactive compound) generated by irradiation with light. As the photoreactive group, one having an unsaturated bond, particularly a double bond, is preferred because the effects of the present invention are more excellent, and examples of the photoreactive group include a group having at least one selected from the group consisting of a carbon-carbon double bond (C=C bond), a carbon-nitrogen double bond (C=N bond), a nitrogen-nitrogen double bond (N=N bond), and a carbon-oxygen double bond (C=O bond).
[0042] Examples of the photoreactive group having a C=C bond include a vinyl group, a polyene group, a stilbene group, a stilbazolium group, a chalcone group, and a cinnamoyl group. Examples of photoreactive groups having a C=N bond include groups having structures such as aromatic Schiff bases and aromatic hydrazones. Examples of the photoreactive group having a C=O bond include a benzophenone group, a coumarin group, an anthraquinone group, and a maleimide group. Examples of photoreactive groups having an N=N bond (hereinafter also referred to as "azo groups") include azobenzene groups, azonaphthalene groups, aromatic heterocyclic azo groups, bisazo groups, and formazan groups, as well as groups having an azoxybenzene basic structure. These groups may have a substituent such as an alkyl group, an alkoxy group, an aryl group, an allyloxy group, a cyano group, an alkoxycarbonyl group, a hydroxyl group, a sulfonic acid group, or a halogenated alkyl group.
[0043] Among these groups, a cinnamoyl group or an azobenzene group is preferred because the amount of polarized light irradiation required for photo-alignment is relatively small and a photo-alignment layer having excellent thermal stability and stability over time is easily obtained.
[0044] (1) Preferred embodiment 1: Photoactive compound having an azobenzene group As the photoactive compound having an azobenzene group, a photoactive compound characterized by being represented by the following general formula (I) is particularly preferred.
[0045] General formula (I) [ka]
[0046] In the formula, R 21 ~R 24 each independently represents a hydrogen atom or a substituent, provided that R 21 ~R 24 represents a carboxyl group or a sulfo group; m represents an integer of 1 to 4, n represents an integer of 1 to 4, o represents an integer of 1 to 5, and p represents an integer of 1 to 5, provided that when m, n, o, and p each represent an integer of 2 or more, there are a plurality of groups represented by R 21 ~R 24 may be the same or different.
[0047] In general formula (I), R 21 ~R 24 Examples of the substituent represented by each of the following formulas can be mentioned: Carboxyl group (which may form a salt with an alkali metal, and is preferably a carboxyl group that does not form a salt or that forms a sodium salt, and more preferably a carboxyl group that forms a sodium salt), sulfo group (which may form a salt with an alkali metal, and is preferably a sulfo group that does not form a salt or that forms a sodium salt, and more preferably a sulfo group that forms a sodium salt), alkyl group (preferably an alkyl group having 1 to 20 carbon atoms, more preferably an alkyl group having 1 to 12 carbon atoms, and particularly preferably an alkyl group having 1 to 8 carbon atoms, and examples thereof include a methyl group, an ethyl group, an isopropyl group, a tert-butyl group, an n-octyl group, an n-decyl group, an n-hexadecyl group, a cyclopropyl group, a cyclopentyl group, and a cyclohexyl group), alkenyl group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 12 carbon atoms, and particularly preferably having 2 alkenyl groups having from 2 to 8 carbon atoms, for example, a vinyl group, an aryl group, a 2-butenyl group, a 3-pentenyl group, etc.), alkynyl groups (preferably alkynyl groups having from 2 to 20 carbon atoms, more preferably 2 to 12 carbon atoms, and particularly preferably 2 to 8 carbon atoms, for example, a propargyl group, a 3-pentynyl group, etc.), aryl groups (preferably aryl groups having from 6 to 30 carbon atoms, more preferably 6 to 20 carbon atoms, and particularly preferably 6 to 12 carbon atoms, for example, a phenyl group, a 2,6-diethylphenyl group, a 3,5-ditrifluoromethylphenyl group, a naphthyl group, a biphenyl group, etc.), substituted or unsubstituted amino groups (preferably amino groups having from 0 to 20 carbon atoms, more preferably 0 to 10 carbon atoms, and particularly preferably 0 to 6 carbon atoms, for example, an unsubstituted amino group, a methylamino group, a dimethylamino group, a diethylamino group, an anilino group, etc.),
[0048] Examples of such an alkoxy group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; examples include a methoxy group, an ethoxy group, and a butoxy group), an alkoxycarbonyl group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and particularly preferably having 2 to 6 carbon atoms; examples include a methoxycarbonyl group and an ethoxycarbonyl group), an acyloxy group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and particularly preferably having 2 to 6 carbon atoms; examples include an acetoxy group and a benzoyloxy group), an acylamino group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and particularly preferably having 2 to 6 carbon atoms; examples include an acetylamino group and a benzoylamino group), an alkoxycarbonylamino group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and particularly preferably having 2 to 6 carbon atoms; examples include a methoxycarbonylamino group). an aryloxycarbonylamino group (preferably having 7 to 20 carbon atoms, more preferably having 7 to 16 carbon atoms, and particularly preferably having 7 to 12 carbon atoms; for example, a phenyloxycarbonylamino group), a sulfonylamino group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; for example, a methanesulfonylamino group, a benzenesulfonylamino group), a sulfamoyl group (preferably having 0 to 20 carbon atoms, more preferably having 0 to 10 carbon atoms, and particularly preferably having 0 to 6 carbon atoms; for example, a sulfamoyl group, a methylsulfamoyl group, a dimethylsulfamoyl group, a phenylsulfamoyl group), a carbamoyl group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; for example, an unsubstituted carbamoyl group, a methylcarbamoyl group, a diethylcarbamoyl group, a phenylcarbamoyl group),
[0049] Alkylthio groups (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; examples include a methylthio group and an ethylthio group), arylthio groups (preferably having 6 to 20 carbon atoms, more preferably having 6 to 16 carbon atoms, and particularly preferably having 6 to 12 carbon atoms; examples include a phenylthio group), sulfonyl groups (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; examples include a mesyl group and a tosyl group), sulfinyl groups (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; examples include a methanesulfinyl group and a benzenesulfinyl group), ureido groups (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; examples include an unsubstituted ureido group, a methylureido group, a phenylureido group), phosphoric acid amide groups (preferably Preferably, the carbon number is 1 to 20, more preferably 1 to 10, and particularly preferably 1 to 6, and examples thereof include a diethylphosphoramide group and a phenylphosphoramide group), a hydroxy group, a mercapto group, a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom), a cyano group, a nitro group, a hydroxamic acid group, a sulfino group, a hydrazino group, an imino group, a heterocyclic group (preferably a heterocyclic group having 1 to 30, more preferably 1 to 12, and examples thereof include a nitrogen atom, heterocyclic group having a heteroatom such as a nitrogen atom, oxygen atom or sulfur atom, examples of which include an imidazolyl group, a pyridyl group, a quinolyl group, a furyl group, a piperidyl group, a morpholino group, a benzoxazolyl group, a benzimidazolyl group, a benzthiazolyl group, etc.), and a silyl group (preferably a silyl group having 3 to 40 carbon atoms, more preferably a silyl group having 3 to 30 carbon atoms, particularly preferably a silyl group having 3 to 24 carbon atoms, examples of which include a trimethylsilyl group and a triphenylsilyl group).
[0050] These substituents may be further substituted with other substituents. When there are two or more substituents, they may be the same or different. If possible, they may be bonded to each other to form a ring. 21 ~R24 The group represented by the formula (I) may be a polymerizable group or a substituent containing a polymerizable group.
[0051] In general formula (I), R 21 ~R 24 The group represented by the formula (I) is preferably a hydrogen atom, a carboxyl group, a sulfo group, a halogen atom, an alkyl group, an alkoxy group, a cyano group, a nitro group, an alkoxycarbonyl group, or a carbamoyl group, more preferably a hydrogen atom, a carboxyl group, a sulfo group, a halogen atom, a halogenated methyl group, a halogenated methoxy group, a cyano group, a nitro group, or a methoxycarbonyl group, and particularly preferably a hydrogen atom, a carboxyl group, a sulfo group, a halogen atom, a cyano group, or a nitro group, because the effects of the present invention are more excellent.
[0052] R 21 ~R 24 At least one of the groups represented by the formula (I) is a carboxyl group or a sulfo group. There is no particular restriction on the substitution position of the carboxyl group or the sulfo group, but from the viewpoint of photoactivity, at least one of the groups represented by the formula (I) is a carboxyl group or a sulfo group. 21 and / or at least one R 22 is preferably a sulfo group, and at least one R 21 and at least one R 22 From the same viewpoint, it is more preferable that at least one R 23 and / or at least one R 24 is preferably a carboxyl group, and at least one R 23 and at least one R 24 More preferably, R is a carboxyl group. The carboxyl group is substituted at the meta position with respect to the azo group. 23 and R 24 It is even more preferable that:
[0053] In general formula (I), m represents an integer of 1 to 4, n represents an integer of 1 to 4, o represents an integer of 1 to 5, and p represents an integer of 1 to 5. Preferably, m is an integer of 1 to 2, n is an integer of 1 to 2, o is an integer of 1 to 2, and p is an integer of 1 to 2.
[0054] Specific examples of the compound represented by formula (I) are given below, but the compound is not limited to these specific examples.
[0055] [ka]
[0056] In the present invention, because of the excellent degree of orientation, the compound having an azo group (particularly, an azobenzene group) having a nitrogen-nitrogen double bond (N=N bond) is preferably a low molecular weight compound having no polymerizable group and a molecular weight of 1000 or less, such as those represented by E-1 to E-17 described above.
[0057] (2) Preferred embodiment 2: Photoactive compound having a cinnamoyl group On the other hand, the photoactive compound having a cinnamoyl group is preferably a polymer, since it is less affected by contact with the photoalignment layer. In addition, the polymer preferably has a crosslinkable group in addition to a cinnamoyl group, since this further reduces the influence of contact with the photoalignment layer. The crosslinkable group may be any group that undergoes a crosslinking reaction to form a crosslink, and examples thereof include cationic polymerizable groups such as epoxy groups; radical polymerizable groups such as acrylate and methacrylate; and the like. On the other hand, in order to improve adhesion, it is more preferable that the hardened film of the photoalignment layer has both a cationic polymerizable group and a radical polymerizable group, since these groups can be used with separate functions.
[0058] A suitable example of a polymer having a crosslinkable group together with a cinnamoyl group is a photoalignable copolymer having a repeating unit A containing a cinnamoyl group represented by the following formula (A) and a repeating unit B containing a crosslinkable group represented by the following formula (B).
[0059] [ka]
[0060] In the above formula (A), R 1 represents a hydrogen atom or a methyl group. 1 represents a divalent linking group containing a nitrogen atom and a cycloalkane ring, and some of the carbon atoms constituting the cycloalkane ring may be substituted with a heteroatom selected from the group consisting of nitrogen, oxygen, and sulfur. R 2 , R 3 , R 4 , R 5 and R 6 each independently represents a hydrogen atom or a substituent, R 2 , R 3 , R 4 , R 5 and R 6 Among these, two adjacent groups may be bonded to form a ring. In the above formula (B), R 7 represents a hydrogen atom or a methyl group, and L 2 represents a divalent linking group, and X represents a crosslinkable group.
[0061] In the present invention, by using a photoalignable copolymer having a repeating unit A containing a cinnamoyl group represented by the above formula (A) and a repeating unit B containing a crosslinkable group represented by the above formula (B), the solvent resistance of the obtained photoalignment layer and the orientation of the polymer liquid crystalline compound when forming the light absorption anisotropic layer (hereinafter abbreviated as "liquid crystal orientation") are improved. Although the details of this are not clear, the present inventors speculate as follows. That is, L in the above formula (A) 1 It is believed that the divalent linking group represented by the formula (I) contains a nitrogen atom and a cycloalkane ring, which enhances hydrogen bonding and molecular rigidity, thereby suppressing molecular motion, thereby improving solvent resistance. Similarly, L in the above formula (A) 1 It is believed that because the divalent linking group represented by the formula (I) contains a nitrogen atom and a cycloalkane ring, the glass transition temperature of the copolymer is increased and the stability over time of the obtained photoalignment layer is improved, resulting in good liquid crystal alignment properties regardless of the timing of forming the optically anisotropic layer.
[0062] Next, L in the above formula (A) 1 The divalent linking group containing a nitrogen atom and a cycloalkane ring represented by the formula (I) will be described. In the present invention, as described above, a part of the carbon atoms constituting the cycloalkane ring may be substituted with a heteroatom selected from the group consisting of nitrogen, oxygen, and sulfur. In addition, when a part of the carbon atoms constituting the cycloalkane ring is substituted with a nitrogen atom, it is not necessary to have a nitrogen atom in addition to the cycloalkane ring.
[0063] In addition, L in the above formula (A) 1 The cycloalkane ring contained in the divalent linking group represented by the formula (I) is preferably a cycloalkane ring having 6 or more carbon atoms, and specific examples thereof include a cyclohexane ring, a cycloheptane ring, a cyclooctane ring, a cyclododecane ring, and a cyclodocosane ring.
[0064] In the present invention, L in the above formula (A) is preferably 0.01 to 0.15 because the liquid crystal alignment property is improved. 1 but, It is preferably a divalent linking group represented by any one of the following formulas (1) to (10).
[0065] [ka]
[0066] In the above formulas (1) to (10), *1 represents the bonding position to the carbon atom constituting the main chain in the above formula (A), and *2 represents the bonding position to the carbon atom constituting the carbonyl group in the above formula (A).
[0067] Among the divalent linking groups represented by any of the above formulas (1) to (10), a divalent linking group represented by any of the above formulas (2), (3), (7) and (8) is preferred because it provides a good balance between the solubility in the solvent used in forming the photo-alignment layer and the solvent resistance of the resulting photo-alignment layer.
[0068] Next, R in the above formula (A) 2, R 3 , R 4 , R 5 and R 6 The substituent represented by one embodiment of the formula (A) will be described below. 2 , R 3 , R 4 , R 5 and R 6 However, as described above, it may be a hydrogen atom instead of a substituent.
[0069] R in the above formula (A) 2 , R 3 , R 4 , R 5 and R 6 The substituents represented by one embodiment of the formula (11) are preferably each independently a halogen atom, a linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, a linear halogenated alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, an aryl group having 6 to 20 carbon atoms, an aryloxy group having 6 to 20 carbon atoms, a hydroxy group, a cyano group, an amino group, or a group represented by the following formula (11), because the cinnamoyl group is more likely to interact with the liquid crystal compound, resulting in better liquid crystal alignment. na - or -O-(CH2) na It may contain a linking group represented by -. na represents an integer of 1 to 10.
[0070] [ka]
[0071] In the above formula (11), * represents the bonding position to the benzene ring in the above formula (A), R 9 represents a monovalent organic group.
[0072] Examples of halogen atoms include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and among these, a fluorine atom and a chlorine atom are preferred.
[0073] Regarding the linear, branched or cyclic alkyl group having 1 to 20 carbon atoms, the linear alkyl group is preferably an alkyl group having 1 to 6 carbon atoms, and specifically, for example, a methyl group, Examples include an ethyl group and an n-propyl group. As the branched alkyl group, an alkyl group having 3 to 6 carbon atoms is preferable, and specific examples thereof include an isopropyl group and a tert-butyl group. The cyclic alkyl group is preferably an alkyl group having 3 to 6 carbon atoms, and specific examples include a cyclopropyl group, a cyclopentyl group, and a cyclohexyl group.
[0074] As the linear halogenated alkyl group having 1 to 20 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms is preferable. Specific examples thereof include a trifluoromethyl group, a perfluoroethyl group, a perfluoropropyl group, and a perfluorobutyl group. Of these, a trifluoromethyl group is preferable.
[0075] As the alkoxy group having 1 to 20 carbon atoms, an alkoxy group having 1 to 18 carbon atoms is preferable. An alkoxy group having 6 to 18 carbon atoms is more preferable, and an alkoxy group having 6 to 14 carbon atoms is even more preferable. Specifically, suitable examples include a methoxy group, an ethoxy group, an n-butoxy group, a methoxyethoxy group, an n-hexyloxy group, an n-octyloxy group, an n-decyloxy group, an n-dodecyloxy group, and an n-tetradecyloxy group, and among these, an n-hexyloxy group, an n-octyloxy group, an n-decyloxy group, an n-dodecyloxy group, and an n-tetradecyloxy group are more preferable.
[0076] As the aryl group having 6 to 20 carbon atoms, an aryl group having 6 to 12 carbon atoms is preferable. Specific examples include a phenyl group, an α-methylphenyl group, and a naphthyl group, and among these, a phenyl group is preferable.
[0077] As the aryloxy group having 6 to 20 carbon atoms, an aryloxy group having 6 to 12 carbon atoms is preferable. Specific examples include a phenyloxy group and a 2-naphthyloxy group, and among these, the phenyloxy group is preferable.
[0078] Examples of the amino group include a primary amino group (-NH2); a secondary amino group such as a methylamino group; and a tertiary amino group such as a dimethylamino group, a diethylamino group, a dibenzylamino group, or a group having a nitrogen atom of a nitrogen-containing heterocyclic compound (e.g., pyrrolidine, piperidine, piperazine, etc.) as a bond.
[0079] Regarding the group represented by the above formula (11), R 9 Examples of the monovalent organic group represented by the formula (I) include alkyl groups having 1 to 20 carbon atoms, and preferred examples include linear alkyl groups having 1 to 20 carbon atoms or cyclic alkyl groups having 3 to 20 carbon atoms. As the linear alkyl group having 1 to 20 carbon atoms, an alkyl group having 1 to 6 carbon atoms is preferable. Specific examples include a methyl group, an ethyl group, and an n-propyl group, and among these, a methyl group or an ethyl group is preferable. As the cyclic alkyl group having 3 to 20 carbon atoms, an alkyl group having 3 to 6 carbon atoms is preferable. Specific examples thereof include a cyclopropyl group, a cyclopentyl group, and a cyclohexyl group. Among them, The cyclohexyl group is preferred. In addition, R in the above formula (11) 9 The monovalent organic group represented by may be a combination of the above-mentioned linear alkyl groups and cyclic alkyl groups either directly or via a single bond.
[0080] In the present invention, the cinnamoyl group is easily interacted with the liquid crystal compound, and the liquid crystal alignment property is improved. For this reason, R 2 , R 3 , R 4 , R 5 and R 6 Of which, At least R 4represents the above-mentioned substituent, and further, for the reasons that the linearity of the obtained photoalignable copolymer is improved, the interaction with the liquid crystal compound becomes easy, and the liquid crystal alignment property becomes further improved, R 2 , R 3 , R 5 and R 6 More preferably, each of represents a hydrogen atom.
[0081] In the present invention, the reaction efficiency is improved when the obtained photo-alignment layer is irradiated with light. R in the above formula (A) 4 is preferably an electron donating substituent. Here, the electron-donating substituent (electron-donating group) refers to a substituent having a Hammett value (Hammett substituent constant σp) of 0 or less, and examples of the substituents mentioned above include an alkyl group, a halogenated alkyl group, and an alkoxy group. Among these, an alkoxy group is preferable, and an alkoxy group having 6 to 16 carbon atoms is more preferable, and an alkoxy group having 7 to 10 carbon atoms is even more preferable, because this leads to better liquid crystal alignment properties.
[0082] Next, L in the above formula (B) 2 The divalent linking group represented by will be described.
[0083] The divalent linking group is preferably a divalent linking group formed by combining at least two or more groups selected from the group consisting of a linear, branched or cyclic alkylene group having 1 to 18 carbon atoms which may have a substituent, an arylene group having 6 to 12 carbon atoms which may have a substituent, an ether group (-O-), a carbonyl group (-C(=O)-), and an imino group (-NH-) which may have a substituent, because the cinnamoyl group easily interacts with the liquid crystal compound and the liquid crystal alignment becomes better.
[0084] Examples of the substituent that the alkylene group, arylene group and imino group may have include a halogen atom, an alkyl group, an alkoxy group, an aryl group, an aryloxy group, a cyano group, a carboxy group, an alkoxycarbonyl group and a hydroxyl group. Examples of halogen atoms include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom, and among these, a fluorine atom and a chlorine atom are preferred. The alkyl group is, for example, preferably a linear, branched or cyclic alkyl group having 1 to 18 carbon atoms, more preferably an alkyl group having 1 to 8 carbon atoms (for example, a methyl group, an ethyl group, a propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a t-butyl group, a cyclohexyl group, etc.), still more preferably an alkyl group having 1 to 4 carbon atoms, and particularly preferably a methyl group or an ethyl group. The alkoxy group is, for example, preferably an alkoxy group having 1 to 18 carbon atoms, more preferably an alkoxy group having 1 to 8 carbon atoms (for example, a methoxy group, an ethoxy group, an n-butoxy group, a methoxyethoxy group, etc.), still more preferably an alkoxy group having 1 to 4 carbon atoms, and particularly preferably a methoxy group or an ethoxy group. Examples of the aryl group include aryl groups having 6 to 12 carbon atoms. Specific examples of the aryl group include Examples include a phenyl group, an α-methylphenyl group, and a naphthyl group, and among these, a phenyl group is preferable. Examples of the aryloxy group include phenoxy, naphthoxy, imidazoyloxy, Examples of the aryloxy group include benzimidazoyloxy, pyridin-4-yloxy, pyrimidinyloxy, quinazolinyloxy, purinyloxy, and thiophen-3-yloxy. Examples of the alkoxycarbonyl group include methoxycarbonyl and ethoxycarbonyl.
[0085] Regarding the linear, branched or cyclic alkylene group having 1 to 18 carbon atoms, specific examples of the linear alkylene group include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a decylene group, an undecylene group, a dodecylene group, a tridecylene group, a tetradecylene group, a pentadecylene group, a hexadecylene group, a heptadecylene group, and an octadecylene group. Specific examples of branched alkylene groups include a dimethylmethylene group, a methylethylene group, a 2,2-dimethylpropylene group, and a 2-ethyl-2-methylpropylene group. Specific examples of the cyclic alkylene group include a cyclopropylene group, a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, a cyclooctylene group, a cyclodecylene group, an adamantane-diyl group, a norbornane-diyl group, and an exo-tetrahydrodicyclopentadiene-diyl group. Of these, a cyclohexylene group is preferable.
[0086] Specific examples of the arylene group having 6 to 12 carbon atoms include a phenylene group, a xylylene group, a biphenylene group, a naphthylene group, and a 2,2'-methylenebisphenyl group, and among these, a phenylene group is preferable.
[0087] Next, the crosslinkable group represented by X in the above formula (B) will be described.
[0088] Specific examples of X (crosslinkable group) in the above formula (B) include an epoxy group, an epoxycyclohexyl group, an oxetanyl group, and a functional group having an ethylenically unsaturated double bond, and among these, at least one type of crosslinkable group selected from the group consisting of the following formulae (X1) to (X4) is preferred. [ka] In the above formulas (X1) to (X4), * represents L in the above formula (B). 2 represents the bond position with R 8represents a hydrogen atom, a methyl group, or an ethyl group, and in the above formula (X4), S represents a functional group having an ethylenically unsaturated double bond. Specific examples of the functional group having an ethylenically unsaturated double bond include a vinyl group, an allyl group, a styryl group, an acryloyl group, and a methacryloyl group, with an acryloyl group or a methacryloyl group being preferred.
[0089] In the present invention, for reasons of increasing the strength of the obtained optical laminate and improving the handleability when forming other layers using the obtained optical laminate, it is preferred that the repeating unit B contains a repeating unit in which X in the above formula (B) is a crosslinkable group represented by any one of the above formulas (X1) to (X3) (hereinafter also abbreviated as "repeating unit B1"), and a repeating unit in which X in the above formula (B) is a crosslinkable group represented by the above formula (X4) (hereinafter also abbreviated as "repeating unit B2").
[0090] Specific examples of the repeating unit A containing a cinnamoyl group represented by the above formula (A) include the repeating units A-1 to A-44 shown below. In the following formula, Me represents a methyl group, and Et represents an ethyl group. In the following specific examples, the "1,4-cyclohexyl group" contained in the divalent linking group of the repeating units A-1 to A-10 may be either a cis or trans form, but is preferably a trans form.
[0091] [ka] JPEG0007578708000008.jpg45142 JPEG0007578708000009.jpg36147 JPEG0007578708000010.jpg39143 [ka] JPEG0007578708000012.jpg53123 JPEG0007578708000013.jpg43131 JPEG0007578708000014.jpg39127 JPEG0007578708000015.jpg39103 JPEG0007578708000016.jpg4787
[0092] On the other hand, specific examples of the repeating unit B (repeating unit B1) containing a crosslinkable group represented by the above formula (B) include repeating units B-1 to B-17 shown below.
[0093] [ka] JPEG0007578708000018.jpg37126 JPEG0007578708000019.jpg39124
[0094] Specific examples of the repeating unit B (repeating unit B2) containing a crosslinkable group represented by the above formula (B) include repeating units B-18 to B-47 shown below. [ka] JPEG0007578708000021.jpg44148 JPEG0007578708000022.jpg31147 JPEG0007578708000023.jpg23148
[0095] In the above-mentioned photoalignable copolymer, it is preferable that the content a of the above-mentioned repeating unit A and the content b of the above-mentioned repeating unit B satisfy the following formula (12) in terms of mass ratio, it is more preferable that they satisfy the following formula (13), it is even more preferable that they satisfy the following formula (14), and it is particularly preferable that they satisfy the following formula (15). 0.03 ≦ a / (a+b) ≦ 0.5 ···(12) 0.03 ≦ a / (a+b) ≦ 0.3 ···(13) 0.03 ≦ a / (a+b) ≦ 0.2 ···(14) 0.05 ≦ a / (a+b) ≦ 0.2 ···(15)
[0096] Furthermore, when the above-mentioned photo-alignable copolymer has the above-mentioned repeating unit B2 in addition to the above-mentioned repeating unit B1, in order to maintain good liquid crystal alignment and adhesion while further increasing the strength of the optically anisotropic layer including the photo-alignment layer, it is preferable that the content a of the above-mentioned repeating unit A, the content b1 of the above-mentioned repeating unit B1, and the content b2 of the above-mentioned repeating unit B2 satisfy the following formula (16) in terms of mass ratio, more preferably the following formula (17), and even more preferably the following formula (18). 0.05 ≦ b2 / (a+b1+b2) ≦ 0.7 ···(16) 0.10 ≦ b2 / (a+b1+b2) ≦ 0.5 ···(17) 0.12 ≦b2 / (a+b1+b2) ≦ 0.35 ···(18)
[0097] The photoalignable copolymer may contain repeating units other than the repeating units A and B described above, as long as the effects of the present invention are not impaired. Examples of monomers (radical polymerizable monomers) that form such other repeating units include: For example, acrylic acid ester compounds, methacrylic acid ester compounds, maleimide compounds, Examples of the compound include an acrylamide compound, an acrylonitrile, a maleic anhydride, a styrene compound, and a vinyl compound.
[0098] The method for synthesizing the photoalignable copolymer is not particularly limited, and the copolymer can be synthesized, for example, by mixing a monomer forming the repeating unit A described above, a monomer forming the repeating unit B described above, and a monomer forming any other repeating unit, and polymerizing the mixture in an organic solvent using a radical polymerization initiator.
[0099] The weight average molecular weight (Mw) of the photoalignable copolymer is preferably from 10,000 to 500,000, and more preferably from 30,000 to 300,000, because this further improves the liquid crystal alignment property.
[0100] When the above-mentioned photo-alignable copolymer is used, the content of the above-mentioned photo-alignable copolymer in the composition for forming a photo-alignment layer is not particularly limited, but when an organic solvent is contained, it is preferably 0.1 to 50 parts by mass, and more preferably 0.5 to 10 parts by mass, per 100 parts by mass of the organic solvent.
[0101] (Additives) The photo-alignment layer forming composition may contain one or more additives other than the photoactive compound. For example, the additive is added for the purpose of adjusting the refractive index of the photo-alignment layer forming composition. As the additive, a compound having a hydrophilic group and a (meth)acryloyloxy group is preferable from the viewpoint of compatibility with the photoactive compound, and it can be added to an extent that does not significantly reduce the alignment ability. Examples of the hydrophilic group include a hydroxyl group, a carboxyl group, a sulfo group, and an amino group. As another example, the additive is added for the purpose of adjusting the elastic modulus of the photo-alignment layer. Examples of the additive include a crosslinking agent, a filler, and a plasticizer. Among them, it is preferable to use a crosslinking agent from the viewpoint of not lowering the alignment ability, and it is preferable that the crosslinking group of the crosslinking agent can react with the crosslinking group of the photoactive compound. It is also preferable that the crosslinking agent has a plurality of crosslinking groups in one molecule.
[0102] (Crosslinking agent) Examples of the crosslinking agent include a compound having two or more epoxy groups or oxetanyl groups in the molecule, a blocked isocyanate compound (a compound having a protected isocyanato group), and an alkoxymethyl group-containing compound. Among these, preferred are compounds having two or more epoxy groups or oxetanyl groups in the molecule and blocked isocyanate compounds, specific examples of which are shown below.
[0103] (1) Compounds having two or more epoxy groups in the molecule Specific examples of compounds having two or more epoxy groups in the molecule include aliphatic epoxy compounds. These are commercially available. For example, Denacol EX-611, EX-612, EX-614, EX-614B, EX-622, EX-512, EX-521, EX-411, EX-421, EX-313, EX-314, EX-321, EX-211, EX-212, EX-810, EX-811, EX-850, EX-851, EX-821, EX-830, EX-832, EX-841, EX-911, EX-941, EX-920, EX-931, EX-212L, EX-214L, EX-216L, EX-321L, EX-85 0L, DLC-201, DLC-203, DLC-204, DLC-205, DLC-206, DLC-301, DLC-402 (all manufactured by Nagase ChemteX Corporation), Celloxide 2021P, 2081, 3000, EHPE3150, Epolead GT401, Cellvinars B0134, B0177 (manufactured by Daicel Corporation), IPU-22G (manufactured by Okamura Oil Mills Co., Ltd.), jERYX7105, jERYX7110, jERYX7400, jERYX7180BH40 (manufactured by Mitsubishi Chemical Corporation), and the like. These can be used alone or in combination of two or more.
[0104] (2) Compounds having two or more oxetanyl groups in the molecule Specific examples of compounds having two or more oxetanyl groups in the molecule include Aron Oxetane OXT-121, OXT-221, OX-SQ, and PNOX (all manufactured by Toagosei Co., Ltd.).
[0105] (3) Blocked isocyanate compounds The blocked isocyanate compound is not particularly limited as long as it is a compound having a blocked isocyanate group in which the isocyanate group is chemically protected. From the viewpoint of curability, however, it is preferable that the blocked isocyanate compound has two or more blocked isocyanate groups in one molecule. In the present invention, the blocked isocyanate group is a group capable of generating an isocyanate group by heat, and a preferred example of the blocked isocyanate group is a group in which an isocyanate group is protected by reacting a blocking agent with the isocyanate group. The blocked isocyanate group is preferably a group capable of generating an isocyanate group by heat of 90°C to 250°C. The skeleton of the blocked isocyanate compound is not particularly limited, and any compound having two isocyanate groups in one molecule may be used. The blocked isocyanate compound may be an aliphatic, alicyclic, or aromatic polyisocyanate. Examples of the blocked isocyanate compound include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 1,3-trimethylene diisocyanate, 1,4-tetramethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, 2,4,4-trimethylhexamethylene diisocyanate, 1,9-nonamethylene diisocyanate, 1,10-decamethylene diisocyanate, 1,4-cyclohexane diisocyanate, 2,2'-diethyl ether diisocyanate, diphenyl diisocyanate, and the like. Isocyanate compounds such as dimethylmethane-4,4'-diisocyanate, o-xylylene diisocyanate, m-xylylene diisocyanate, p-xylylene diisocyanate, methylenebis(cyclohexylisocyanate), cyclohexane-1,3-dimethylene diisocyanate, cyclohexane-1,4-dimethylene diisocyanate, 1,5-naphthalene diisocyanate, p-phenylene diisocyanate, 3,3'-methylene d-tolylene-4,4'-diisocyanate, 4,4'-diphenyl ether diisocyanate, tetrachlorophenylene diisocyanate, norbornane diisocyanate, hydrogenated 1,3-xylylene diisocyanate, and hydrogenated 1,4-xylylene diisocyanate, as well as prepolymer-type skeleton compounds derived from these compounds, can be suitably used. Among these, tolylene diisocyanate (TDI), diphenylmethane diisocyanate (MDI), hexamethylene diisocyanate (HDI), and isophorone diisocyanate (IPDI) are particularly preferred.
[0106] Examples of the parent structure of the blocked isocyanate compound include a biuret type, an isocyanurate type, an adduct type, and a bifunctional prepolymer type. Examples of blocking agents that form a block structure of the blocked isocyanate compound include oxime compounds, lactam compounds, phenol compounds, alcohol compounds, amine compounds, active methylene compounds, pyrazole compounds, mercaptan compounds, imidazole compounds, imide compounds, etc. Among these, blocking agents selected from oxime compounds, lactam compounds, phenol compounds, alcohol compounds, amine compounds, active methylene compounds, and pyrazole compounds are particularly preferred.
[0107] The blocked isocyanate compound is available as a commercially available product, for example, Coronate AP Stable M, Coronate 2503, 2515, 2507, 2513, 2555, Millionate MS-50 (all manufactured by Nippon Polyurethane Industry Co., Ltd.), Takenate B-830, B-815N, B-820NSU, B-842N, B-846N, B-870N, B-874N , B-882N (all manufactured by Mitsui Chemicals, Inc.), Duranate 17B-60PX, 17B-60P, TPA-B80X, TPA-B80E, MF-B60X, MF-B60B, MF-K60X, MF-K60B, E402-B80B, SBN-70D, SBB-70P, K6000 (all manufactured by Asahi Kasei Chemicals Corp.), Desmodur BL1100, BL1265 MPA / X, BL3575 / 1, BL3272MPA, BL3370MPA, BL3475BA / SN, BL5375MPA, VPLS2078 / 2, BL4265SN, PL340, PL350, Sumidur BL3175 (all manufactured by Sumika Bayer Urethane Co., Ltd.), and the like can be preferably used.
[0108] (4)Content When the composition for forming a photoalignment layer contains a crosslinking agent, the content is not particularly limited. However, because the effects of the present invention are more excellent, the content is preferably 1 to 300 parts by mass, and more preferably 10 to 100 parts by mass, relative to 100 parts by mass of the above-mentioned photoactive compound.
[0109] The composition for forming a photoalignment layer may contain other components in addition to those described above, and examples thereof include a crosslinking catalyst (for example, a thermally reactive acid generator), an adhesion improver, a leveling agent, and a surfactant.
[0110] When the additive is used for the purpose of adjusting the refractive index of the composition for forming a photo-alignment layer, the refractive index of the additive is preferably from 1.4 to 1.6, and more preferably from 1.4 to 1.55.
[0111] (Organic solvent) From the viewpoint of workability in producing the photoalignment layer, the composition for forming the photoalignment layer preferably contains an organic solvent. Specific examples of the organic solvent include ketones (e.g., acetone, 2-butanone, methyl isobutyl ketone, cyclohexanone, cyclopentanone, etc.), ethers (e.g., dioxane, tetrahydrofuran, etc.), aliphatic hydrocarbons (e.g., hexane, etc.), alicyclic hydrocarbons (e.g., cyclohexane, etc.), aromatic hydrocarbons (e.g., toluene, xylene, trimethylbenzene, etc.), halogenated carbons (e.g., dichloromethane, dichloroethane, dichlorobenzene, chlorotoluene, etc.), esters (e.g., methyl acetate, ethyl acetate, butyl acetate, etc.), water, alcohols (e.g., ethanol, isopropanol, butanol, cyclohexanol, etc.), cellosolves (e.g., methyl cellosolve, ethyl cellosolve, etc.), cellosolve acetates, sulfoxides (e.g., dimethyl sulfoxide, etc.), amides (e.g., dimethylformamide, dimethylacetamide, etc.), and the like. These may be used alone or in combination of two or more.
[0112] In the present invention, because the adhesion between the photo-alignment layer and the light absorption anisotropic layer is good, it is preferable that the composition for forming the photo-alignment layer contains a compound having a photoreactive group and a crosslinkable group (e.g., the above-mentioned photo-alignment copolymer, etc.) and does not contain a radical polymerization initiator.
[0113] (Application method) As a method for applying the composition for forming a photoalignment layer onto the above-mentioned polymer film, a known method such as a coating method such as a spin coating method, an extrusion method, a gravure coating method, a die coating method, a bar coating method, or an applicator method, or a printing method such as a flexography method can be used. When the optical laminate is produced by a continuous production method of a roll-to-roll type, the coating method usually used is a printing method such as a gravure coating method, a die coating method or a flexography method.
[0114] <Drying process> The method for drying the coating film formed in the coating step by heating is not particularly limited, and the drying temperature is preferably in the range of 50 to 180°C, more preferably in the range of 80 to 150°C. The drying time is preferably from 10 seconds to 10 minutes, and more preferably from 30 seconds to 5 minutes. When the composition for forming a photoalignment layer contains a crosslinking catalyst such as a heat-reactive acid generator and a compound having a cationic polymerizable crosslinking group, it is preferable to proceed with curing through a crosslinking reaction of the coating film by heat in this step.
[0115] <Light irradiation process> There are no particular limitations on the polarized light to be irradiated onto the coating film after the drying step. Examples include linearly polarized light, circularly polarized light, and elliptically polarized light, and among these, linearly polarized light is preferred. Furthermore, the "oblique direction" in which the unpolarized light is irradiated is not particularly limited as long as it is a direction inclined at a polar angle θ (0<θ<90°) with respect to the normal direction to the coating surface, and can be appropriately selected depending on the purpose, but it is preferable that θ is 20 to 80°. In this specification, "irradiation with linearly polarized light" and "irradiation with non-polarized light" are operations for causing a photoreaction in a photoactive compound. The wavelength of the light used varies depending on the photoactive compound used, and is not particularly limited as long as it is a wavelength necessary for the photoreaction. The peak wavelength of the light used for photoirradiation is preferably 200 nm to 700 nm, and more preferably ultraviolet light with a peak wavelength of 400 nm or less.
[0116] Examples of light sources used for light irradiation include commonly used light sources, such as lamps such as tungsten lamps, halogen lamps, xenon lamps, xenon flash lamps, mercury lamps, mercury xenon lamps, and carbon arc lamps, various lasers [e.g., semiconductor lasers, helium-neon lasers, argon ion lasers, helium cadmium lasers, and YAG (yttrium-aluminum-garnet) lasers], light-emitting diodes, and cathode ray tubes.
[0117] As a means for obtaining linearly polarized light, a method using a polarizing plate (e.g., an iodine polarizing plate, a dichroic dye polarizing plate, and a wire grid polarizing plate), a method using a prism-based element (e.g., a Glan-Thompson prism) or a reflective polarizer using the Brewster angle, or a method using light emitted from a polarized laser light source can be adopted. Also, a filter or a wavelength conversion element or the like may be used to selectively irradiate only light of a required wavelength.
[0118] In the case of linearly polarized light, the light is irradiated from the top or back surface of the alignment layer perpendicularly or obliquely to the alignment layer surface. The incident angle of the light varies depending on the photoactive compound, but is preferably 0 to 90° (perpendicular), more preferably 40 to 90°. In the case of non-polarized light, the alignment layer is irradiated with non-polarized light obliquely, preferably at an incident angle of 10 to 80°, more preferably at 20 to 60°, and even more preferably at 30 to 50°. The irradiation time is preferably from 1 minute to 60 minutes, and more preferably from 1 minute to 10 minutes.
[0119] When patterning is required, a method of irradiating light using a photomask the number of times required to form a pattern, or a method of writing a pattern by laser light scanning can be used.
[0120] The photo-alignment layer used in the present invention is preferably an alignment layer having an average refractive index of 1.55 to 1.8 at a wavelength of 550 nm. From the viewpoint of further improving the anti-reflection performance, in order to reduce the difference in refractive index with the light absorptive anisotropic layer, the average refractive index at a wavelength of 550 nm is more preferably 1.55 to 1.7.
[0121] The photo-alignment layer used in the present invention preferably has an in-plane refractive index anisotropy Δn at a wavelength of 550 nm of 0.05 to 0.45, more preferably 0.1 to 0.4, and even more preferably 0.1 to 0.3. By appropriately controlling the refractive index anisotropy of the photo-alignment layer, the anti-reflection function can be further improved.
[0122] <Rubbing Treatment Alignment Layer> The rubbed alignment layer is a layer to which an alignment control force is imparted by a rubbing treatment. The polymer materials used for the rubbing treatment alignment layer are described in many documents, and many commercial products are available. In the present invention, polyvinyl alcohol or polyimide and its derivatives are preferably used. For the alignment layer, the description on page 43, line 24 to page 49, line 8 of International Publication WO01 / 88574A1 can be referred to.
[0123] [Thickness of resin layer] The thickness d of the resin layer is preferably 10 μm or less, more preferably 5 μm or less, further preferably 3 μm or less, and particularly preferably 2 μm or less, for reasons of superior effect of the present invention. The thickness d of the resin layer is preferably 0.01 μm or more, and more preferably 0.1 μm or more.
[0124] [Storage modulus Ea of resin layer] The storage modulus Ea of the resin layer is not particularly limited as long as it satisfies the above-mentioned formula (1-1). However, in order to obtain better effects of the present invention, it is preferably 1 GPa or more and 10 GPa or less, and more preferably 1 GPa or more and 5 GPa or less.
[0125] The method for controlling the storage modulus Ea of the resin layer is not particularly limited, but examples thereof include a method for changing the type of compound forming the resin layer, a method for incorporating a crosslinking agent into the composition for forming the resin layer, and a method for changing the conditions for light irradiation, if any.
[0126] [Light-absorbing anisotropic layer] The light absorption anisotropic layer of the specific laminate is a layer containing a dichroic material and having anisotropy in light absorption.
[0127] From the viewpoint of further increasing the anisotropy of absorption, the light absorption anisotropic layer is preferably a light absorption anisotropic layer formed by applying a liquid crystal composition containing a dichroic substance and a polymer liquid crystal compound. As the light absorption anisotropic layer of such an embodiment, the polarizing layer described in paragraphs
[0079] to
[0215] of International Publication No. 2020 / 179864 can be suitably exemplified.
[0128] [Thickness of Light Absorption Anisotropic Layer] The thickness of the optically absorptive anisotropic layer is preferably 5 μm or less, more preferably 0.1 to 5.0 μm, and even more preferably 0.3 to 2.0 μm.
[0129] [Hardened layer] The specific laminate may have a cured layer having a thickness of 100 nm or less for the purpose of reducing the refractive index difference between the light absorption anisotropic layer and the adjacent layer. It is preferable that the cured layer is provided on the side opposite to the resin layer (particularly the photo-alignment layer) of the light absorption anisotropic layer. Such a cured layer is not particularly limited, and various known layers can be used. For example, a layer containing a liquid crystal compound or a layer obtained by curing a composition containing a polyfunctional monomer can be used. It is preferable that the cured layer has a refractive index that can be index-matched with the light absorption anisotropic layer.
[0130] [Oxygen barrier layer] The specific laminate may have an oxygen barrier layer for the purpose of improving light resistance. It is preferable that the oxygen barrier layer is provided on the side of the light absorption anisotropic layer opposite to the resin layer (particularly the photoalignment layer). Here, the oxygen barrier layer refers to an oxygen barrier film having an oxygen barrier function, and specific examples include layers containing organic compounds such as polyvinyl alcohol, polyethylene vinyl alcohol, polyvinyl ether, polyvinylpyrrolidone, polyacrylamide, polyacrylic acid, cellulose ether, polyamide, polyimide, styrene / maleic acid copolymer, gelatin, vinylidene chloride, and cellulose nanofibers.
[0131] In this specification, the oxygen barrier function is not limited to a state in which no oxygen passes through, but also includes a state in which some oxygen passes through depending on the desired performance.
[0132] When an oxygen-barrier layer is provided on a transparent polymer film and a photo-alignment layer having an azobenzene compound represented by the general formula (I) is provided on the oxygen-barrier layer, it is preferable to use polyvinyl alcohol having a saponification degree of 95 mol % or more or modified polyvinyl alcohol having a saponification degree of 95 mol % or more for the oxygen-barrier layer in order to enhance alignment.
[0133] Also included are thin layers made of metal compounds (metal compound thin layers). Any method can be used to form the metal compound thin layer as long as it can form the desired thin layer. For example, sputtering, vacuum deposition, ion plating, and plasma CVD (Chemical Vapor Deposition) are suitable, and specifically, the methods described in Japanese Patent No. 3400324, JP-A-2002-322561, and JP-A-2002-361774 can be used.
[0134] The components contained in the metal compound thin layer are not particularly limited as long as they can exhibit an oxygen blocking function, and for example, oxides, nitrides, or oxynitrides containing one or more metals selected from Si, Al, In, Sn, Zn, Ti, Cu, Ce, Ta, etc. can be used. Among these, oxides, nitrides, or oxynitrides of metals selected from Si, Al, In, Sn, Zn, and Ti are preferred, and metal oxides, nitrides, or oxynitrides selected from Si, Al, Sn, and Ti are particularly preferred. These may contain other elements as secondary components.
[0135] The oxygen barrier layer may be in the form of a laminate of a layer containing the above-mentioned organic material and a thin layer of a metal compound, as described in, for example, U.S. Pat. No. 6,413,645, JP 2015-226995 A, JP 2013-202971 A, JP 2003-335880 A, JP 53-12953 A, and JP 58-217344 A, or may be a hybrid layer of an organic compound and an inorganic compound, as described in WO 2011 / 11836 A, JP 2013-248832 A, and Japanese Patent No. 3,855,004.
[0136] When the optical laminate of the present invention has a λ / 4 plate described later, and the λ / 4 plate is a retardation film having an optically anisotropic layer having λ / 4 function provided on a support, the oxygen barrier layer may also serve as an orientation layer for the optically anisotropic layer having λ / 4 function. In such a case, the oxygen barrier layer is preferably an oxygen barrier layer containing polyvinyl alcohol, polyamide, or polyimide.
[0137] [Thickness of oxygen barrier layer] The thickness of the oxygen barrier layer is not particularly limited, but in the case of a layer containing an organic compound, the thickness is preferably 0.1 to 10 μm, more preferably 0.5 to 5.5 μm, because the effect of the present invention is more excellent. In the case of a thin metal compound layer, the thickness of the oxygen barrier layer is preferably 5 nm to 500 nm, more preferably 10 nm to 200 nm, because the effect of the present invention is more excellent.
[0138] The specific laminate may have an optically anisotropic layer (retardation layer) other than the optically absorptive anisotropic layer. For example, the optically absorptive anisotropic layer adjacent to the optical alignment layer may have an optically anisotropic layer on the surface facing the optical alignment layer. For example, it is more preferable to have at least one optically absorptive anisotropic layer and at least one retardation layer, and it is even more preferable to be composed of an optically absorptive anisotropic layer and a λ / 4 plate.
[0139] [Specific laminate thickness] The thickness of the specific laminate is preferably 0.1 to 10 μm, and more preferably 1 to 5 μm, because the effects of the present invention are more excellent.
[0140] [3] Surface protective layer The laminate of the present invention may have a surface protective layer on the most visible side. The surface protective layer is not limited as long as it has the function of protecting the surface. It may be a single layer, but multiple layers are also preferred. It is also preferred that the hardness is high, but it is also preferred that the recovery is high. A low reflection layer that suppresses surface reflection occurring at the air interface is also preferred. A preferred embodiment is a structure consisting of a transparent support and a surface coating layer. The transparent support and the surface coating layer will be described below.
[0141] [Transparent support] The laminate of the present invention may have a transparent support. Here, the term "transparent" in the present invention indicates that the transmittance of visible light is 60% or more, preferably 80% or more, and particularly preferably 90% or more. Specific examples of the transparent support include a glass substrate and a plastic substrate, and among these, a plastic substrate is preferable. Examples of plastics constituting the plastic substrate include polyolefins such as polyethylene, polypropylene, and norbornene-based polymers; cyclic olefin-based resins; polyvinyl alcohol; polyethylene terephthalate; polymethacrylic acid esters; polyacrylic acid esters; cellulose esters such as triacetyl cellulose (TAC), diacetyl cellulose, and cellulose acetate propionate; polyethylene naphthalate; polycarbonate; polysulfone; polyether sulfone; polyether ketone; polyphenylene sulfide; polyphenylene oxide, and polyimide. Among these, cellulose esters, cyclic olefin-based resins, polyethylene terephthalate, and polymethacrylic acid esters are particularly preferred because they are easily available on the market and have excellent transparency. From the viewpoint of flexibility, polyimides are superior. Polyimides have a high refractive index and may have a large refractive index gap, but it is also preferable to adjust the refractive index by a method such as mixing silica particles. Details of polyimides are described in International Publication No. WO 2018 / 062296 and International Publication No. WO 2018 / 062190.
[0142] The thickness of the transparent support is preferably thin enough to maintain strength and processability, in order to provide a mass that allows practical handling and to ensure sufficient transparency. The thickness of the glass substrate is preferably from 100 to 3000 μm, and more preferably from 100 to 1000 μm. The thickness of the plastic substrate is preferably from 5 to 300 μm, and more preferably from 5 to 200 μm. When the laminate of the present invention is used as a circular polarizing plate (particularly when used as a circular polarizing plate for mobile devices), the transparent support preferably has a thickness of about 5 to 100 μm.
[0143] [Surface coating layer] The surface coating layer may be at least one selected from the group consisting of an anti-reflection layer, an anti-glare layer, and a hard coating layer. These layers may be made of known layer materials. These layers may be laminated in a plurality of layers.
[0144] The anti-reflection layer is different from the so-called circular polarizer anti-reflection plate, and refers to a structure that reduces reflection by using a structure that uses light interference. The anti-reflection layer may be composed of only a low refractive index layer as the simplest configuration. In order to further reduce the reflectance, it is preferable to configure the anti-reflection layer by combining a high refractive index layer with a low refractive index layer with a low refractive index. Configuration examples include a two-layer structure of a high refractive index layer / low refractive index layer from the bottom, and a structure in which three layers with different refractive indices are stacked in the order of a medium refractive index layer (a layer with a higher refractive index than the lower layer and a lower refractive index than the high refractive index layer) / a high refractive index layer / a low refractive index layer, and a structure in which even more anti-reflection layers are stacked has also been proposed. Among them, in terms of durability, optical properties, cost, productivity, etc., it is preferable to have a medium refractive index layer / high refractive index layer / low refractive index layer in this order on the hard coat layer, and examples of such structures include those described in JP-A-8-122504, JP-A-8-110401, JP-A-10-300902, JP-A-2002-243906, and JP-A-2000-111706. In addition, a three-layer antireflection film with excellent robustness against film thickness fluctuations is described in JP-A-2008-262187. When the above three-layer antireflection film is installed on the surface of an image display device, the average reflectance can be set to 0.5% or less, reflection can be significantly reduced, and an image with excellent three-dimensional effect can be obtained. In addition, each layer may be given other functions, such as an antifouling low refractive index layer, an antistatic high refractive index layer, an antistatic hard coat layer, and an antiglare hard coat layer (e.g., JP-A-10-206603, JP-A-2002-243906, JP-A-2007-264113, etc.). As one embodiment of the present invention, the description of JP 2018-56069 A can be used as a reference for a foldable organic EL display device other than a polarizer. Since a cover glass cannot be used, a surface film is required. For example, in
[0030] to
[0040] , it is described that a polyimide-based resin is preferable as a substrate having a bending property that can be folded preferably 200,000 times, more preferably 300,000 times, and even more preferably 500,000 times with a curvature radius of 3 mm or less (for example, 3 mm, 2 mm, 1 mm), and that an organic-inorganic hybrid material in which silica particles or a cage-shaped silsesquioxane compound is blended with an ultraviolet-curable acrylic resin is preferable as a hard coat layer. In the surface layer of the present invention, a hard coat using a silsesquioxane compound having a structure described in JP-A-2015-212353, JP-A-2017-008148, or the like is preferable.
[0145] [4]λ / 4 plate The optical laminate of the present invention may have a λ / 4 plate on the side of the pressure-sensitive adhesive layer 1 opposite to the specific laminate. Here, the term "λ / 4 plate" refers to a plate having a λ / 4 function, specifically, a plate having the function of converting linearly polarized light of a certain wavelength into circularly polarized light (or circularly polarized light into linearly polarized light). A specific example of a λ / 4 plate is described in, for example, US Patent Application Publication No. 2015 / 0277006. For example, specific examples of the λ / 4 plate having a single layer structure include a stretched polymer film and a retardation film having an optically anisotropic layer having λ / 4 function provided on a support, and specific examples of the λ / 4 plate having a multilayer structure include a broadband λ / 4 plate formed by laminating a λ / 4 plate and a λ / 2 plate. It is more preferable that the retardation film having an optically anisotropic layer having λ / 4 function is a retardation film having one or more layers containing at least one liquid crystal compound (disk-shaped liquid crystal, rod-shaped liquid crystal compound, etc.) formed by polymerizing a liquid crystal monomer that produces a nematic liquid crystal layer or a smectic liquid crystal layer. It is also more preferable to use a liquid crystal compound with reverse wavelength dispersion as a λ / 4 plate with excellent optical performance. Specifically, a liquid crystal compound of general formula (II) described in International Publication No. WO2017 / 043438 is preferably used. For a method of producing a λ / 4 plate using a liquid crystal compound with reverse wavelength dispersion, the description of Examples 1 to 10 of WO2017 / 043438 and Example 1 of JP-A-2016-91022 can be referred to.
[0146] [5] Functional layer The laminate of the present invention or the specific laminate described above preferably has a functional layer having a function of reducing shortwave light on the viewing side of the light absorption anisotropic layer. By reducing shortwave light, photodecomposition of the dye compound can be suppressed, and an optical laminate having excellent light resistance can be provided. In one embodiment, the pressure-sensitive adhesive layer or the oxygen barrier layer preferably has a function of reducing shortwave light. In another embodiment, it is also preferable to provide a new layer having a function of reducing short wave light on the viewing side of the optically anisotropic layer (particularly the light absorptive anisotropic layer).
[0147] The method for reducing shortwave light is not particularly limited, and examples thereof include a method using light absorption by an absorbent or the like, and a method using wavelength selective reflection by a multilayer film.
[0148] The aforementioned shortwave light refers to light with a wavelength of 430 nm or less. By reducing the amount of light with a wavelength of 430 nm or less, it is possible to suppress the photodecomposition of coloring compounds caused by sunlight or the light source used in the light resistance tests of JIS B 7751 and JIS B 7754. In order not to affect the performance of the polarizer in visible light, it is preferable that the film is transparent in the wavelength region of 450 nm or more.
[0149] [6]Applications The optical laminate of the present invention can be used, for example, as a polarizing element (polarizing plate), specifically, for example, as a linear polarizing plate or a circular polarizing plate (particularly for antireflection).
[0150] [II] Image display device The image display device of the present invention has the above-mentioned optical layered body of the present invention. The display element used in the image display device of the present invention is not particularly limited, and examples thereof include a liquid crystal cell, an organic electroluminescence (hereinafter abbreviated as "EL") display panel, and a plasma display panel. Among these, a liquid crystal cell or an organic EL display panel is preferred, and an organic EL display panel is more preferred. That is, the image display device of the present invention is preferably a liquid crystal display device using a liquid crystal cell as a display element, or an organic EL display device using an organic EL display panel as a display element, and more preferably an organic EL display device.
[0151] [1] Liquid crystal display device A liquid crystal display device, which is one example of the image display device of the present invention, is a liquid crystal display device having the above-mentioned optical laminate of the present invention (however, not including a λ / 4 plate) and a liquid crystal cell. In the present invention, of the optical laminates provided on both sides of the liquid crystal cell, it is preferable to use the optical laminate of the present invention as the polarizing element on the front side (viewing side), and it is more preferable to use the optical laminate of the present invention as the polarizing elements on the front side and the rear side. The liquid crystal cell constituting the liquid crystal display device will be described in detail below.
[0152] [Liquid crystal cell] The liquid crystal cell used in the liquid crystal display device is preferably in VA (Vertical Alignment) mode, OCB (Optically Compensated Bend) mode, IPS (In-Plane-Switching) mode, or TN (Twisted Nematic) mode, but is not limited to these. In a TN mode liquid crystal cell, rod-shaped liquid crystal molecules (rod-shaped liquid crystal compounds) are aligned substantially horizontally when no voltage is applied, and are further aligned in a twisted manner at an angle of 60 to 120°. TN mode liquid crystal cells are most commonly used as color TFT liquid crystal display devices, and are described in many publications. In a VA mode liquid crystal cell, rod-shaped liquid crystal molecules are aligned substantially vertically when no voltage is applied. VA mode liquid crystal cells include (1) narrowly defined VA mode liquid crystal cells in which rod-shaped liquid crystal molecules are aligned substantially vertically when no voltage is applied and substantially horizontally when voltage is applied (described in Japanese Patent Laid-Open Publication No. 2-176625), (2) multi-domain VA mode (MVA mode (Multi-domain Vertical Alignment)) liquid crystal cells in which VA mode is multi-domained to widen the viewing angle (described in SID97, Digest of tech. Papers (Proceedings) 28 (1997) 845), (3) n-ASM (Axially symmetric aligned microcell) mode liquid crystal cells in which rod-shaped liquid crystal molecules are aligned substantially vertically when no voltage is applied and substantially horizontally when voltage is applied (described in Proceedings of the Japan Liquid Crystal Discussion Society 58-59 (1998)), and (4) SURVIVAL mode liquid crystal cells (announced at LCD (Liquid Crystal Display) International 98). In addition, the liquid crystal display may be of any of a PVA (Patterned Vertical Alignment) type, an optical alignment type, and a PSA (Polymer-Sustained Alignment) type. Details of these modes are described in detail in Japanese Patent Application Laid-Open No. 2006-215326 and Japanese Patent Application Laid-Open No. 2008-538819. In the IPS mode liquid crystal cell, rod-shaped liquid crystal molecules are aligned substantially parallel to the substrate, and the liquid crystal molecules respond in a planar manner when an electric field parallel to the substrate surface is applied. In the IPS mode, the black display is achieved when no electric field is applied, and the absorption axes of the pair of upper and lower polarizing plates are perpendicular to each other. Methods of reducing light leakage during black display in an oblique direction and improving the viewing angle using an optical compensation sheet are disclosed in JP-A-10-54982, JP-A-11-202323, JP-A-9-292522, JP-A-11-133408, JP-A-11-305217, JP-A-10-307291, and the like.
[0153] [2] Organic EL display device A preferred embodiment of an organic EL display device, which is one example of the image display device of the present invention, includes, from the viewing side, the above-mentioned optical laminate of the present invention (including a pressure-sensitive adhesive layer and a λ / 4 plate) and an organic EL display panel, in this order. The organic EL display panel is a display panel configured using an organic EL element having an organic light-emitting layer (organic electroluminescence layer) sandwiched between electrodes (cathode and anode). The configuration of the organic EL display panel is not particularly limited, and a known configuration may be adopted. EXAMPLES
[0154] The present invention will be described in more detail below based on examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the following examples.
[0155] [Example 1] [Preparation of transparent support] <Preparation of cellulose acylate dope for core layer> The following composition was charged into a mixing tank and stirred to dissolve each component, thereby preparing a cellulose acetate solution to be used as a cellulose acylate dope for the core layer. ------------------------------------------------------------------ Core layer: Cellulose acylate dope ------------------------------------------------------------------ Cellulose acetate with an acetyl substitution degree of 2.88: 100 parts by weight In the embodiment of JP 2015-227955 A 12 parts by weight of the polyester compound B 2 parts by weight of the following compound F Methylene chloride (first solvent) 430 parts by weight Methanol (second solvent) 64 parts by weight ------------------------------------------------------------------
[0156] Compound F [ka]
[0157] <Preparation of outer layer cellulose acylate dope> To 90 parts by weight of the above-mentioned cellulose acylate dope for the core layer, 10 parts by weight of the following matting agent solution was added to prepare a cellulose acetate solution to be used as the cellulose acylate dope for the outer layer.
[0158] ------------------------------------------------------------------ Matting agent solution ------------------------------------------------------------------ Silica particles with an average particle size of 20 nm (AEROSIL R972, manufactured by Nippon Aerosil Co., Ltd.) 2 parts by weight Methylene chloride (first solvent) 76 parts by weight Methanol (second solvent) 11 parts by weight 1 part by weight of the above-mentioned cellulose acylate dope for the core layer ------------------------------------------------------------------
[0159] <Preparation of Cellulose Acylate Film 1> The above core layer cellulose acylate dope and the above outer layer cellulose acylate dope were filtered through a filter paper with an average pore size of 34 μm and a sintered metal filter with an average pore size of 10 μm, and then the above core layer cellulose acylate dope and the outer layer cellulose acylate dope on both sides were simultaneously cast onto a drum at 20°C from a casting nozzle (band casting machine). Next, the film was peeled off while the solvent content was about 20% by mass, and both ends in the width direction of the film were fixed with tenter clips, and the film was stretched in the transverse direction at a stretch ratio of 1.1 times while being dried. Thereafter, the film was further dried by being conveyed between rolls of a heat treatment device, to prepare an optical film (transparent support) having a thickness of 40 μm.
[0160] [Formation of Resin Layer A1] The following resin layer-forming coating liquid A1 was continuously applied onto the cellulose acylate film 1 using a wire bar. The support on which the coating film was formed was dried with hot air at 140°C for 120 seconds to form a resin layer A1, thereby obtaining a TAC (triacetyl cellulose) film with a resin layer. The resin layer A1 had a thickness of 2.5 μm. The resin layer A1 had a storage modulus Ea of 4.2 GPa. The resin layer A1 had a wet heat distortion Δa of 0.48%.
[0161] ------------------------------------------------------------------ Resin layer forming coating solution A1 ------------------------------------------------------------------ 69.20 parts by weight of the photo-alignment polymer PA-1 below 10.38 parts by weight of the following acid generator: San-Aid SI-B3A - 0.42 parts by weight of the following stabilizer DIPEA Xylene 828.00 parts by weight Methyl isobutyl ketone 92.00 parts by weight ------------------------------------------------------------------
[0162] Photoalignment film polymer PA-1 (wherein the numerical value for each repeating unit represents the content (mass%) of each repeating unit relative to the total repeating units.) [ka]
[0163] Acid generator San-Aid SI-B3A [ka]
[0164] Stabilizer DIPEA [ka]
[0165] [Preparation of optically absorbing anisotropic film P1] The resin layer A1 thus obtained was irradiated with polarized ultraviolet light (10 mJ / cm 2 After the substrate was irradiated with light (using an ultra-high pressure mercury lamp) to develop photoalignment ability, a composition P1 for forming an optically absorptive anisotropic film having the following composition was continuously applied with a wire bar to form a coating layer P1. Next, the coating layer P1 was heated at 140° C. for 15 seconds, and then cooled to room temperature (23° C.). The coating layer P1 was then heated at 75° C. for 60 seconds and cooled again to room temperature. After that, an LED lamp (center wavelength 365 nm) was used to illuminate the sample at an intensity of 200 mW / cm 2 The resin layer A1 was irradiated for 2 seconds under the irradiation conditions described above to form an optically absorptive anisotropic film P1 on the resin layer A1. The optically absorptive anisotropic film P1 had a film thickness of 0.5 μm.
[0166] ------------------------------------------------------------------ Optically absorptive anisotropic film forming composition P1 ------------------------------------------------------------------ 0.59 parts by weight of the following first dichroic substance C-1 0.36 parts by weight of the second dichroic substance M-1 below 0.24 parts by weight of the following third dichroic material Y-1 5.55 parts by weight of the following liquid crystal compound L-1 Polymerization initiator IRGACUREOXE-02 (BASF) 0.21 parts by mass 0.055 parts by weight of the following surfactant F-1 Cyclopentanone 45.34 parts by mass Tetrahydrofuran 45.34 parts by weight Benzyl alcohol 2.33 parts by weight ------------------------------------------------------------------
[0167] Dichroic substance C-1 (maximum absorption wavelength: 570 nm) [ka]
[0168] Dichroic substance M-1 (maximum absorption wavelength: 466 nm) [ka]
[0169] Dichroic substance Y-1 (maximum absorption wavelength: 417 nm) [ka]
[0170] Liquid crystal compound L-1 (wherein the numerical values for each repeating unit ("59", "15", "26") represent the content (mass%) of each repeating unit relative to the total repeating units.) [ka]
[0171] Surfactant F-1 (wherein the numerical value for each repeating unit represents the content (mass%) of each repeating unit relative to the total repeating units.) [ka]
[0172] [Formation of oxygen barrier layer B1] A coating solution B1 having the following composition was continuously applied onto the optically absorptive anisotropic film P1 using a wire bar. After that, the coating solution was dried for 5 minutes using hot air at 80°C to obtain a laminate A having an oxygen barrier layer B1 of 1.0 μm thickness made of polyvinyl alcohol (PVA), that is, a laminate A having a cellulose acylate film 1 (transparent support), a resin layer A1, an optically absorptive anisotropic film P1, and an oxygen barrier layer B1 adjacent to each other in this order. The transmittance of the obtained laminate A in the wavelength range of 280 to 780 nm was measured using a spectrophotometer, and the average visible light transmittance was 48%.
[0173] ------------------------------------------------------------------ Oxygen barrier layer forming coating solution B1 ------------------------------------------------------------------ 3.80 parts by weight of the following modified polyvinyl alcohol Initiator Irg2959 0.20 parts by weight ·Water 70 parts by mass Methanol 30 parts by weight ------------------------------------------------------------------
[0174] Modified Polyvinyl Alcohol [ka]
[0175] [Preparation of TAC film A1 with positive A plate A1] The coating solution PA1 for forming a photo-alignment film having the following composition was continuously coated on the above-mentioned cellulose acylate film 1 using a wire bar. The support on which the coating film was formed was dried with hot air at 140° C. for 120 seconds, and then the coating film was irradiated with polarized ultraviolet light (10 mJ / cm 2 By using an ultra-high pressure mercury lamp), a photo-alignment film PA1 having a thickness of 0.2 μm was formed, and a TAC film with a photo-alignment film was obtained.
[0176] ------------------------------------------------------------------ Coating liquid PA1 for photo alignment film formation ------------------------------------------------------------------ 100.00 parts by weight of the following photo-alignment film polymer PA-2 5.00 parts by weight of the following acid generator PAG-1 0.005 parts by weight of the following acid generator CPI-110F Isopropyl alcohol 16.50 parts by weight Butyl acetate 1072.00 parts by weight Methyl ethyl ketone 268.00 parts by mass ------------------------------------------------------------------
[0177] Photo-aligned polymer PA-2 [ka]
[0178] Acid generator PAG-1 [ka]
[0179] Acid generator CPI-110F [ka]
[0180] Composition A-1 having the following composition was applied onto the photo-alignment film PA1 using a bar coater. The coating film formed on the photo-alignment film PA1 was heated to 120°C with hot air, then cooled to 60°C, and then irradiated with 100 mJ / cm2 at a wavelength of 365 nm using a high-pressure mercury lamp under a nitrogen atmosphere. 2 The coating was then irradiated with 500 mJ / cm2 of ultraviolet light, followed by heating to 120°C. 2 The coating film was irradiated with ultraviolet light of 1000 nm to fix the alignment of the liquid crystal compound, thereby preparing a TAC film A1 having a positive A plate A1. The positive A plate A1 had a thickness of 2.5 μm and Re(550) of 144 nm. The positive A plate A1 also satisfied the relationship Re(450)≦Re(550)≦Re(650). Re(450) / Re(550) was 0.82.
[0181] ------------------------------------------------------------------ Composition A-1 ------------------------------------------------------------------ 43.50 parts by weight of the following polymerizable liquid crystal compound LA-1 43.50 parts by weight of the following polymerizable liquid crystal compound LA-2 8.00 parts by weight of the following polymerizable liquid crystal compound LA-3 5.00 parts by weight of the following polymerizable liquid crystal compound LA-4 0.55 parts by weight of the following polymerization initiator PI-1 0.20 parts by weight of the following leveling agent T-1 Cyclopentanone 235.00 parts by mass ------------------------------------------------------------------
[0182] Polymerizable liquid crystal compound LA-1 (tBu represents a tertiary butyl group) [ka]
[0183] Polymerizable liquid crystal compound LA-2 [ka]
[0184] Polymerizable liquid crystal compound LA-3 [ka]
[0185] Polymerizable liquid crystal compound LA-4 (Me represents a methyl group) [ka]
[0186] Polymerization initiator PI-1 [ka]
[0187] Leveling agent T-1 [ka]
[0188] [Preparation of TAC film C1 with positive C-plate C1] As the temporary support, the above-mentioned cellulose acylate film 1 was used. The cellulose acylate film 1 was passed through a dielectric heating roll at a temperature of 60° C. to raise the film surface temperature to 40° C., and then an alkaline solution having the composition shown below was applied to one side of the film in an amount of 14 ml / m using a bar coater. 2 The mixture was heated to 110° C. and conveyed under a steam type far-infrared heater manufactured by Noritake Co., Ltd. for 10 seconds. Next, using the same bar coater, pure water was applied onto the film at a rate of 3 ml / m 2 It was applied. Next, after washing with water using a fountain coater and draining with an air knife were repeated three times, the film was transported to a drying zone at 70° C. for 10 seconds and dried to prepare an alkaline saponified cellulose acylate film 1.
[0189] ------------------------------------------------------------------ (Alkaline solution) ------------------------------------------------------------------ Potassium hydroxide 4.7 parts by weight ·Water 15.8 parts by mass 63.7 parts by weight of isopropanol Surfactant SF-1 (C 14 H 29 O(CH2CH2O) 20 H) 1.0 parts by mass Propylene glycol 14.8 parts by weight ------------------------------------------------------------------
[0190] An alignment film-forming coating solution PA2 having the following composition was continuously applied using a #8 wire bar onto the above-mentioned alkaline saponification-treated cellulose acylate film 1. The obtained film was dried with hot air at 60° C. for 60 seconds and then with hot air at 100° C. for 120 seconds to form an alignment film PA2.
[0191] ------------------------------------------------------------------ Alignment film forming coating solution PA2 ------------------------------------------------------------------ Polyvinyl alcohol (Kuraray, PVA103) 2.4 parts by weight Isopropyl alcohol 1.6 parts by weight Methanol 36 parts by weight ·Water 60 parts by mass ------------------------------------------------------------------
[0192] A coating solution C1 for forming a positive C plate having the following composition was applied onto the alignment film PA2, and the resulting coating film was aged at 60° C. for 60 seconds, and then irradiated with 70 mW / cm 2 in air. 2 An air-cooled metal halide lamp (manufactured by Eye Graphics Co., Ltd.) was used, and the output was 1000 mJ / cm 2 The alignment state was fixed by irradiating the liquid crystal compound with ultraviolet light of 1000 nm to vertically align the liquid crystal compound, thereby preparing a TAC film C1 having a positive C plate C1 with a thickness of 0.5 μm. The Rth(550) of the obtained positive C plate was −60 nm.
[0193] ------------------------------------------------------------------ Positive C-plate coating solution C1 ------------------------------------------------------------------ 80 parts by weight of the following liquid crystal compound LC-1 20 parts by weight of the following liquid crystal compound LC-2 1 part by weight of the following vertical alignment liquid crystal compound promoter S01 Ethylene oxide modified trimethylolpropane triacrylate (V#360, manufactured by Osaka Organic Chemical Co., Ltd.) 8 parts by mass Irgacure 907 (BASF) 3 parts by weight Kayacure DETX (manufactured by Nippon Kayaku Co., Ltd.) 1 part by weight 0.4 parts by mass of the following compound B03 Methyl ethyl ketone 170 parts by weight Cyclohexanone 30 parts by weight ------------------------------------------------------------------
[0194] Liquid crystal compound LC-1 [ka]
[0195] Liquid crystal compound LC-2 [ka]
[0196] Vertical alignment liquid crystal compound promoter S01 [ka]
[0197] Compound B03 [ka]
[0198] [Preparation of UV adhesive composition] The following UV adhesive composition was prepared. ───────────────────────────────── UV adhesive composition ------------------------------------------------------------------ CEL2021P (manufactured by Daicel) 70 parts by weight 1,4-butanediol diglycidyl ether 20 parts by weight 2-Ethylhexyl glycidyl ether 10 parts by mass ·CPI-100P 2.25 parts by mass ─────────────────────────────────
[0199] CPI-100P [ka]
[0200] [Preparation of optical laminate of Example 1] The retardation side (positive A plate A1 side) of the TAC film A1 having the positive A plate A1 and the retardation side (positive C plate C1 side) of the TAC film C1 having the positive C plate C1 are bonded to each other with the UV adhesive composition at 600 mJ / cm 2 The plates were laminated together by UV irradiation. The thickness of the UV adhesive layer was 3 μm. The surfaces to be laminated with the UV adhesive were each subjected to a corona treatment. Next, the photo-alignment layer PA1 and the cellulose acylate film 1 on the positive A plate A1 side were removed to obtain a retardation plate 1. The layer structure of the retardation plate 1 was positive A plate A1 / UV adhesive layer / positive C plate C1 / alignment layer PA2 / cellulose acylate film 1. Next, the oxygen barrier layer B1 side of the laminate A was bonded to the support side of a low reflection surface film CV-LC5 (manufactured by Fujifilm Corporation) using Opteria D692 (thickness 15 μm, storage modulus 0.004 GPa, manufactured by Lintec Corporation) as adhesive A. Next, only the cellulose acylate film 1 was removed, and the surface from which it was removed was bonded to the positive A plate A1 side of the retardation plate 1 using the adhesive A to prepare an optical laminate of Example 1. At this time, the layers were bonded so that the angle between the absorption axis of the light absorption anisotropic layer P1 and the slow axis of the positive A plate A1 was 45°. In this way, an optical laminate of Example 1 was obtained, having cellulose acylate film 1, alignment layer PA2, positive C plate C1, UV adhesive layer, positive A plate A1 (λ / 4 plate), adhesive A, resin layer A1, light absorption anisotropic layer P1, oxygen barrier layer B1, adhesive A, and low-reflection surface film CV-LC5 (surface protection layer) adjacent to each other in this order.
[0201] [Examples 2 to 4] An optical laminate was produced in the same manner as in Example 1, except that the resin layer-forming coating liquid A1 was changed to the resin layer-forming coating liquid A2 having the following composition and the thickness of the resin layer was changed to the thickness shown in Table 1 below.
[0202] ------------------------------------------------------------------ Coating liquid A2 for resin layer formation ------------------------------------------------------------------ The above photoalignment film polymer PA-1: 51.53 parts by weight jER YX7400 (Mitsubishi Chemical Corporation) 7.73 parts by weight Epolead GT401 (manufactured by Daicel) 13.40 parts by weight 6.90 parts by weight of the acid generator San-Aid SI-B3A 0.44 parts by weight of the above stabilizer DIPEA Xylene 828.00 parts by weight Methyl isobutyl ketone 92.00 parts by weight ------------------------------------------------------------------
[0203] [Example 5] An optical laminate was produced in the same manner as in Example 1, except that the resin layer-forming coating liquid A1 was changed to the resin layer-forming coating liquid A3 having the following composition and the thickness of the resin layer was changed to the thickness shown in Table 1 below.
[0204] ------------------------------------------------------------------ Resin layer forming coating solution A3 ------------------------------------------------------------------ 49.08 parts by weight of the above photoalignment film polymer PA-1 jER YX7400 (Mitsubishi Chemical Corporation) 7.36 parts by weight Epolead GT401 (manufactured by Daicel) 12.76 parts by weight 10.38 parts by weight of the acid generator San-Aid SI-B3A 0.42 parts by weight of the above stabilizer DIPEA Xylene 828.00 parts by weight Methyl isobutyl ketone 92.00 parts by weight ------------------------------------------------------------------
[0205] [Example 6] An optical laminate was produced in the same manner as in Example 1, except that the resin layer-forming coating liquid A1 was changed to the resin layer-forming coating liquid A4 having the following composition and the film thickness of the resin layer was changed to the film thickness shown in Table 1 below.
[0206] ------------------------------------------------------------------ Resin layer forming coating solution A4 ------------------------------------------------------------------ The above photoalignment film polymer PA-1: 51.53 parts by weight jER YX7400 (Mitsubishi Chemical Corporation) 21.13 parts by weight 6.90 parts by weight of the acid generator San-Aid SI-B3A 0.44 parts by weight of the above stabilizer DIPEA Xylene 828.00 parts by weight Methyl isobutyl ketone 92.00 parts by weight ------------------------------------------------------------------
[0207] [Example 7] An optical laminate was produced in the same manner as in Example 1, except that the coating liquid A1 for forming a resin layer was changed to the coating liquid A5 for forming a resin layer having the following composition, and the adhesive B described below was used when bonding the surface of the laminate A from which the cellulose acylate film 1 had been removed to the positive A plate A1 side of the retardation plate 1.
[0208] ------------------------------------------------------------------ Coating liquid A5 for resin layer formation ------------------------------------------------------------------ 36.33 parts by weight of the above photoalignment film polymer PA-1 jER YX7400 (Mitsubishi Chemical Corporation) 36.33 parts by weight 6.90 parts by weight of the acid generator San-Aid SI-B3A 0.44 parts by weight of the above stabilizer DIPEA Xylene 828.00 parts by weight Methyl isobutyl ketone 92.00 parts by weight ------------------------------------------------------------------
[0209] [Preparation of Adhesive B] First, an acrylic polymer was prepared according to the following procedure. In a reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer, 70 parts by mass of 2-ethylhexyl acrylate, 20 parts by mass of ethyl acrylate, 6 parts by mass of hydroxyethyl methacrylate, and 4 parts by mass of acrylic acid were polymerized by solution polymerization to obtain an acrylic polymer 1 having an average molecular weight of 300,000.
[0210] Next, the obtained acrylic polymer 1 was used to prepare pressure-sensitive adhesive B according to the following procedure. Specifically, 3.83 parts by mass of trimethylolpropane tolylene diisocyanate (Coronate L, manufactured by Nippon Polyurethane Industry Co., Ltd.) was added to 100 parts by mass of the solid content of the acrylic polymer 1 to prepare a pressure-sensitive adhesive composition B. Next, the prepared adhesive composition B was applied to a PET film surface-treated with a silicone-based release agent using a die coater and dried at 150°C for 3 hours to produce an adhesive B having an adhesive layer with a thickness of 15 µm. The storage modulus of the adhesive B was 0.001 GPa.
[0211] [Example 8] An optical laminate was produced in the same manner as in Example 1, except that the coating liquid A1 for forming the resin layer was changed to the coating liquid A6 for forming the resin layer having the following composition, and PD-S1 (thickness 25 μm, storage modulus 0.0005 GPa, manufactured by PANAC Corporation) was used as the adhesive C when bonding the surface of the laminate A from which the cellulose acylate film 1 had been removed to the positive A plate A1 side of the retardation plate 1.
[0212] ------------------------------------------------------------------ Resin layer forming coating solution A6 ------------------------------------------------------------------ 31.46 parts by weight of the above photoalignment film polymer PA-1 jER YX7400 (Mitsubishi Chemical Corporation) 37.75 parts by weight 10.38 parts by weight of the acid generator San-Aid SI-B3A 0.42 parts by weight of the above stabilizer DIPEA Xylene 828.00 parts by weight Methyl isobutyl ketone 92.00 parts by weight ------------------------------------------------------------------
[0213] [Example 9] An optical laminate was produced in the same manner as in Example 1, except that the resin layer-forming coating liquid A1 was changed to the resin layer-forming coating liquid A7 having the following composition and the thickness of the resin layer was changed to the thickness shown in Table 1 below.
[0214] ------------------------------------------------------------------ Resin layer forming coating solution A7 ------------------------------------------------------------------ The above photoalignment film polymer PA-1: 51.53 parts by weight IPU-22G (Okamura Oil Mills) 7.73 parts by weight Epolead GT401 (manufactured by Daicel) 13.40 parts by weight 6.90 parts by weight of the acid generator San-Aid SI-B3A 0.44 parts by weight of the above stabilizer DIPEA Xylene 828.00 parts by weight Methyl isobutyl ketone 92.00 parts by weight ------------------------------------------------------------------
[0215] [Example 10] A laminate B having a cellulose acylate film 1 (transparent support), a resin layer B1, an optically absorptive anisotropic film P1, and an oxygen-blocking layer B1 adjacent to each other in this order was obtained in the same manner as in Example 1, except that the coating liquid A1 for forming a resin layer was changed to a coating liquid B1 for forming a resin layer having the following composition.
[0216] ------------------------------------------------------------------ Resin layer forming coating liquid B1 ------------------------------------------------------------------ Photo-alignment film polymer PA-3 (73.50 parts by weight) 6.06 parts by weight of the acid generator San-Aid SI-B3A 0.44 parts by weight of the above stabilizer DIPEA Butyl acetate 736.00 parts by weight Methyl ethyl ketone 184.00 parts by mass ------------------------------------------------------------------
[0217] Next, in the same manner as in Example 1, a TAC film A1 having a positive A plate A1, a TAC film C1 having a positive C plate C1, and a retardation plate 1 were produced. Next, in preparing an optical laminate in the same manner as in Example 1, the oxygen barrier layer B1 side of the laminate B was bonded to the support side of a low reflection surface film CV-LC5 (manufactured by Fujifilm Corporation) using Opteria D692 (thickness 15 μm, storage modulus 0.004 GPa, manufactured by Lintec Corporation) as the adhesive A, and then the cellulose acylate film 1 and the resin layer B1 of the laminate B were removed together, and the following resin layer forming coating solution A8 was continuously applied to the removed surface with a wire bar, and then dried with hot air at 60° C. for 1 minute, and then subjected to irradiation with an LED lamp (center wavelength 365 nm) at an illuminance of 200 mW / cm 2 By irradiating for 2 seconds under the irradiation conditions, a resin layer A8 having a thickness of 0.4 μm was formed.
[0218] ------------------------------------------------------------------ Resin layer forming coating solution A8 ------------------------------------------------------------------ Acrylit 8KX-078 (manufactured by Taisei Fine Chemical Co., Ltd., solid content 40%) 23.34 parts by mass Polymerization initiator IRGACUREOXE-02 (BASF) 0.28 parts by mass 0.009 parts by weight of the following surfactant F-5 Methyl ethyl ketone 76.37 parts by mass ------------------------------------------------------------------
[0219] Surfactant F-5 [ka]
[0220] Next, the resin layer A8 and the positive A plate A1 side of the retardation plate 1 were bonded together in the same manner as in Example 1 to prepare an optical laminate of Example 10. In this way, an optical laminate was produced having, adjacently in this order, cellulose acylate film 1, alignment layer PA2, positive C plate C1, UV adhesive layer, positive A plate A1 (λ / 4 plate), adhesive A, resin layer A8, light absorption anisotropic layer P1, oxygen barrier layer B1, adhesive A, and low reflection surface film CV-LC5 (surface protection layer).
[0221] [Comparative Example 1] An optical laminate was produced in the same manner as in Example 1, except that the coating liquid A1 for forming a resin layer was changed to the composition PA1 for forming an alignment layer used in Example 7 of Patent Document 1 (International Publication No. 2020 / 080359), and the film thickness of the resin layer (photoalignment layer) was changed to 0.5 μm, the same as in Example 7.
[0222] [Comparative Examples 2 to 3] An optical laminate was produced in the same manner as in Example 1, except that the composition of the resin layer-forming coating liquid and the type of adhesive were changed as shown in Table 1 below.
[0223] [Durability evaluation] The durability of each of the obtained optical laminates was evaluated. Specifically, the optical laminate was cut into a 10 cm square, and then the cellulose acylate film 1 and the alignment layer PA2 were removed to expose the positive C plate C1. The exposed surface of the positive C plate C1 was then bonded to an aluminum substrate using adhesive C, and the plate was then placed in a thermo-hygrostat at 60°C and 90%RH for 65 hours and removed. The surface condition was then visually observed and scored as follows. The surface reflectance of the prepared aluminum substrate was 84%. AA: No uneven reflection was observed after placement in the temperature and humidity chamber. A: After being placed in the temperature and humidity chamber, extremely slight unevenness in reflection was observed. B: Slight unevenness in reflection was observed after placement in the temperature and humidity chamber. C: After being placed in the temperature and humidity chamber, strong uneven reflection was observed. The results are shown in the following Table 1. In practice, AA to B is preferable, and AA is more preferable.
[0224] [Table 1]
[0225] From the results shown in Table 1, it was found that all of the optical laminates in which the storage modulus Ep of the pressure-sensitive adhesive layer 1 and the storage modulus Ea and moist heat distortion Δa of the resin layer satisfy the following formula (1-1) have good durability (Examples 1 to 10). In particular, it was found that the optical laminates satisfying the following formula (1-4) have even better durability. 1 / 4(3×Ep / Ea) 2 / 3 > δa (1-1) 1 / 4(3×Ep / Ea) 2 / 3 -δa ≧ 0.15 (1-4)
[0226] In contrast, it was found that the optical laminate having the resin layer (photo-alignment layer) described in Patent Document 1 has poor durability because the storage modulus Ep of the pressure-sensitive adhesive layer 1 and the storage modulus Ea and moist heat distortion Δa of the resin layer do not satisfy the above formula (1-1) (Comparative Example 1). Furthermore, even when the same resin layer as in Example 1 was used, it was found that the durability was poor when the type of adhesive was different and did not satisfy the above formula (1-1) (Comparative Examples 2 and 3). [Explanation of symbols]
[0227] 1 Adhesive layer 1 2 Adhesive layer 2 20 Resin layer 22 Photoalignment layer 30 Optically Absorbing Anisotropic Layer 40 Specific laminate 42 Specific laminate 50 hardened layer 60 Oxygen barrier layer 70 Surface protective layer 80 λ / 4 plate 100 Optical multilayer 200 Optical multilayer
Claims
1. An optical laminate comprising, in this order, a pressure-sensitive adhesive layer 1, a specific laminate having a resin layer and a light absorption anisotropic layer adjacent to each other, and a pressure-sensitive adhesive layer 2, the light absorption anisotropic layer contains a dichroic material, The pressure-sensitive adhesive layer 1 is adjacent to the resin layer of the specific laminate, The optical laminate, wherein the storage modulus Ep of the pressure-sensitive adhesive layer 1, and the storage modulus Ea and the wet heat distortion δa of the resin layer satisfy the following formula (1-1). 1 / 4 (3×E~~~) 2/3 > δ。 ・・・(1-1) Here, the storage modulus Ep of the pressure-sensitive adhesive layer 1 is in MPa, the storage modulus Ea of the resin layer is in GPa, and the wet heat distortion δa of the resin layer is a value defined by the following formula (2). D max / L 0 ×1000 ・・・(22) L max : Maximum displacement (mm) when the temperature profile in the following wet heat distortion test is applied L 0 : Distance between chucks in the following heat and humidity distortion test (mm) Humid heat distortion test: A single resin layer having a thickness of 10 μm was used as a test specimen, and with a chuck distance of 15 mm and a tensile load of 0.02 mN applied, the specimen was held in an environment of 25° C. and 50% relative humidity for 30 minutes, and then the temperature and humidity were raised to an environment of 60° C. and 90% relative humidity over 80 minutes. Next, the specimen was held in an environment of 60° C. and 90% relative humidity for 120 minutes, and then the temperature and humidity were lowered to 25° C. and 50% relative humidity over 80 minutes.
2. The optical laminate according to claim 1 , wherein the resin layer is an alignment layer.
3. The optical stack according to claim 2 , wherein the alignment layer is a photoalignment layer.
4. The optical laminate according to any one of claims 1 to 3, wherein the storage modulus Ep of the pressure-sensitive adhesive layer 1, the storage modulus Ea and the wet heat distortion δa of the resin layer satisfy the following formula (1-2). 1 / 4 (3×E~~~) 2/3 -δa ≧ 0.15 ・・・(1-2)
5. The optical laminate according to any one of claims 1 to 4, wherein the resin layer has a storage modulus Ea of 1 GPa or more and 10 GPa or less.
6. The optical laminate according to any one of claims 1 to 5, wherein the resin layer has a storage modulus Ea of 1 GPa or more and 5 GPa or less.
7. The optical laminate according to any one of claims 1 to 6, having a thickness of 50 µm or less.
8. The optical laminate according to any one of claims 1 to 7, wherein the resin layer has a thickness of 2 µm or less.
9. An image display device comprising the optical laminate according to any one of claims 1 to 8 and an image display element.
10. The image display device according to claim 9 , which is an organic electroluminescence display device.
Citation Information
Patent Citations
Adhesive composition, manufacturing method therefor, adhesive sheet and image display device
JP2017095660A
Laminate and method for manufacturing the same
JP2020019277A
Light-absorbing anisotropic film, optical layered product, and image display device
WO2019131976A1
Laminate, and image display device